Vane, compressor, and vane manufacturing method
The vane with a nitrided base material and sputtered hard coating on the tip surface addresses wear and seizure issues by enhancing wear resistance and preventing protrusions, reducing piston wear and ensuring effective sliding performance.
Patent Information
- Application Number
- PCT/JP2024/003130
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-01-31
- Publication Date
- 2024-10-03
AI Technical Summary
Existing rotary compressor vanes face wear and seizure issues due to insufficient hardness on the tip surface, which is subjected to high pressure, leading to increased wear when sliding with the piston, despite having adequate wear and seizure resistance on the side and end surfaces.
A vane with a nitrided base material and a hard coating on the tip surface formed by the sputtering method, ensuring wear resistance and seizure resistance while preventing protrusions that could enhance wear on the piston.
The vane effectively reduces wear on the piston while maintaining necessary wear and seizure resistance on the tip surface, preventing abnormal wear due to high surface pressure and ensuring the hard coating adheres well to the dense nitrided layer.
Smart Images

Figure JP2024003130_03102024_PF_FP_ABST
Abstract
Description
Vane, compressor, and method for manufacturing vane
[0001] The present invention relates to a vane, a compressor, and a method for manufacturing the vane.
[0002] The compression section of a rotary compressor includes a cylinder, a piston that revolves along the inner circumferential surface of the cylinder, and a pair of end plates that close both ends of the cylinder. A cylinder chamber is defined by the inner circumferential surface of the cylinder, the outer circumferential surface of the piston, and the pair of end plates. A vane that divides the cylinder chamber into a suction chamber and a compression chamber is disposed in a vane groove formed in the cylinder. The outer circumferential surface of this type of vane has a tip surface that slides against the outer circumferential surface of the piston, a side surface that slides against the inner surface of the vane groove, and an end surface that slides against the end plate. Therefore, the sliding surfaces of the vane (tip surface, side surface, end surface) must be wear-resistant to withstand repeated sliding against the piston and end plate, and seizure-resistant to withstand temperature increases due to frictional heat caused by sliding. The tip surface of the vane, in particular, must be highly hard (wear-resistant) to withstand the pressure exerted by the outer circumferential surface of the piston during sliding contact with the piston.
[0003] JP-A No. 60-26195 JP-A No. 10-159774
[0004] In the rotary compressor described in Patent Document 1, wear resistance and seizure resistance are ensured simply by nitriding vanes formed from a steel material with a high Cr content as a base material to form a nitride diffusion layer on the surface of the vane. However, while the vane described in Patent Document 1 has sufficient wear resistance and seizure resistance on the side and end surfaces, it lacks the hardness required for the tip surface of the vane, which is subjected to a large force from the piston and a large surface pressure due to the small contact area when sliding with the piston, and so there is a risk of wear on the tip surface progressing.
[0005] In the rotary compressor described in Patent Document 2, vanes are nitrided and then a CrN film is formed thereon to improve the vane's wear resistance and seizure resistance. However, when a coating of CrN or the like is formed on the surface of a steel material by ion plating (arc method) as described in Patent Document 2, droplets measuring several tens of microns are generated when the material to be coated is turned into plasma, and these droplets may become trapped in the coating, forming protrusions. If protrusions such as CrN are formed on the tip of the vane, they may be highly aggressive to the piston that slides against the vane, causing wear on the piston surface.
[0006] The disclosed technology has been made in consideration of the above, and aims to provide a vane that reduces piston wear while ensuring the necessary wear resistance and seizure resistance on the tip surface of the vane, a compressor equipped with the vane, and a method for manufacturing the vane.
[0007] One aspect of the vane disclosed in the present application is a vane used in a compressor including a cylinder, a piston that revolves along the inner circumferential surface of the cylinder, and an end plate that closes the end of the cylinder, and which divides a cylinder chamber surrounded by the cylinder, the piston, and the end plate into a suction chamber and a compression chamber. The vane includes a nitrided base material and a hard coating that covers the tip end surface of the base material, and the hard coating is a hard coating formed by a sputtering method.
[0008] According to one aspect of the vane disclosed in the present application, piston wear can be reduced while ensuring the necessary wear resistance and seizure resistance of the tip surface of the vane.
[0009] FIG. 1 is a longitudinal cross-sectional view showing a compressor including a vane according to a first embodiment. FIG. 2 is an exploded perspective view showing a compression section of the compressor according to the first embodiment. FIG. 3 is a perspective view showing a vane according to the first embodiment. FIG. 4 is a cross-sectional view showing a hard coating and a nitride layer of the vane according to the first embodiment. FIG. 5 is an enlarged cross-sectional view showing a tip portion of the vane according to the first embodiment. FIG. 6 is a schematic view for explaining a manufacturing method of the vane according to the first embodiment. FIG. 7 is a cross-sectional view showing the surface of a base material immediately after nitriding. FIG. 8 is a cross-sectional view showing a film-forming apparatus for forming a hard coating on the tip surface of a base material by sputtering. FIG. 9 is a schematic view for explaining an example of a hard coating formation process according to the first embodiment. FIG. 10 is a cross-sectional view showing another film-forming apparatus for forming a hard coating on the tip surface of a vane according to a comparative example by arc ion plating. FIG. 11 is a perspective view showing the surface of a hard coating of a vane according to a comparative example. FIG. 12 is an enlarged cross-sectional view showing the tip portion of a vane according to a second embodiment. FIG. 13 is a schematic view for explaining an example of a hard coating formation process according to the second embodiment.
[0010] A vane, a compressor including the vane, and a method for manufacturing the vane according to embodiments disclosed herein will be described below with reference to the drawings. Note that the following description does not limit the technology of the present disclosure. In addition, in the following description, the same components are given the same reference numerals, and duplicated descriptions will be omitted.
[0011] (Configuration of Compressor) Fig. 1 is a longitudinal cross-sectional view showing a compressor including a vane according to a first embodiment. As shown in Fig. 1, compressor 1 is a rotary compressor that accommodates, inside main container 10, a compression section 12 that draws in refrigerant from an accumulator 25, compresses the refrigerant, and discharges the compressed refrigerant into main container 10, and a motor 11 that drives compression section 12. Compressor 1 discharges high-pressure refrigerant compressed by compression section 12 into main container 10 and further into a refrigeration cycle through a discharge pipe 107. Compressor 1 also includes a rotary shaft 15 that transmits the driving force of motor 11 to compression section 12, and an accumulator 25 fixed to the outer circumferential surface of main container 10.
[0012] An upper compression section suction pipe 102T and a lower compression section suction pipe 102S are provided penetrating the main container 10 for drawing low-pressure refrigerant from the refrigeration cycle into the compression section 12. More specifically, an upper guide pipe 101T is fixed to the main container 10 by, for example, brazing, and the upper compression section suction pipe 102T passes through the inside of the upper guide pipe 101T and is fixed to the upper guide pipe 101T by, for example, brazing. Similarly, a lower guide pipe 101S is fixed to the main container 10 by, for example, brazing, and the lower compression section suction pipe 102S passes through the inside of the lower guide pipe 101S and is fixed to the lower guide pipe 101S by, for example, brazing.
[0013] A discharge pipe 107 for discharging the high-pressure refrigerant compressed in the compression section 12 from inside the main container 10 to the refrigeration cycle is provided through the upper part of the main container 10. A base member 310 for supporting the entire compressor 1 is fixed to the lower part of the main container 10 by welding.
[0014] The accumulator 25 includes an accumulator suction pipe 27 that draws refrigerant from the refrigeration cycle into the accumulator 25, and an upper gas-liquid separation pipe 31T and a lower gas-liquid separation pipe 31S that send the gaseous refrigerant to the compression section 12. The accumulator suction pipe 27 is connected to an upper portion of the accumulator 25. The upper gas-liquid separation pipe 31T is connected to an upper compression section suction pipe 102T via an upper connecting pipe 104T. The lower gas-liquid separation pipe 31S is connected to a lower compression section suction pipe 102S via a lower connecting pipe 104S.
[0015] FIG. 2 is an exploded perspective view showing the compression section 12 of the compressor 1 of the first embodiment. As shown in FIGS. 1 and 2 , the compression section 12 includes an upper cylinder 121T, a lower cylinder 121S, an intermediate partition plate 140, an upper end plate 160T, and a lower end plate 160S. The upper end plate 160T, the upper cylinder 121T, the intermediate partition plate 140, the lower cylinder 121S, and the lower end plate 160S are stacked in this order and secured with a plurality of bolts 175. The upper end plate 160T is provided with a main bearing 161T. The lower end plate 160S is provided with a sub-bearing 161S. The rotating shaft 15 includes a main shaft 153, an upper eccentric portion 152T, a lower eccentric portion 152S, and a sub-shaft 151. The rotating shaft 15 includes the main shaft 153 and the sub-shaft 151 supported by the compression section 12. The main shaft portion 153 of the rotating shaft 15 is fitted into the main bearing portion 161T of the upper end plate 160T, and the sub-shaft portion 151 of the rotating shaft 15 is fitted into the sub-bearing portion 161S of the lower end plate 160S, so that the rotating shaft 15 is rotatably supported by the main bearing portion 161T and the sub-bearing portion 161S.
[0016] The motor 11 has a stator 111 disposed on the outside and a rotor 112 disposed on the inside. The stator 111 is fixed to the inner circumferential surface 10a of the main container 10 by, for example, shrink fitting or welding. The rotor 112 is fixed to the rotating shaft 15 by shrink fitting.
[0017] The interior of the main container 10 is filled with lubricating oil 18 in an amount that nearly immerses the compression section 12, for lubricating the sliding members of the compression section 12 and sealing between the high-pressure and low-pressure sections within the cylinder chamber.
[0018] Next, the compression section 12 will be described in detail using Figure 2. The upper cylinder 121T has a cylindrical upper hollow section 130T therein, and an upper piston 125T is disposed in the upper hollow section 130T. The upper piston 125T is fitted into the upper eccentric section 152T of the rotary shaft 15. The lower cylinder 121S has a cylindrical lower hollow section 130S therein, and a lower piston 125S is disposed in the lower hollow section 130S. The lower piston 125S is fitted into the lower eccentric section 152S of the rotary shaft 15.
[0019] The upper cylinder 121T is provided with an upper vane groove 128T extending from the upper hollow portion 130T to the outer periphery, and an upper vane 127T is disposed in the upper vane groove 128T. The upper cylinder 121T is provided with an upper spring hole 124T that leads from the outer periphery to the upper vane groove 128T, and an upper spring 126T is disposed in the upper spring hole 124T. The lower cylinder 121S is provided with a lower vane groove 128S that extends from the lower hollow portion 130S to the outer periphery, and a lower vane 127S is disposed in the lower vane groove 128S. The lower cylinder 121S is provided with a lower spring hole 124S that leads from the outer periphery to the lower vane groove 128S, and a lower spring 126S is disposed in the lower spring hole 124S.
[0020] One end of the upper vane 127T is pressed against the upper piston 125T by the upper spring 126T, dividing the space outside the upper piston 125T in the upper hollow portion 130T of the upper cylinder 121T into an upper suction chamber 131T and an upper compression chamber 133T, which are upper cylinder chambers. The upper cylinder 121T has an upper suction hole 135T that communicates with the upper suction chamber 131T from its outer periphery. The upper suction hole 135T is connected to an upper compression section suction pipe 102T. One end of the lower vane 127S is pressed against the lower piston 125S by the lower spring 126S, dividing the space outside the lower piston 125S in the lower hollow portion 130S of the lower cylinder 121S into a lower suction chamber 131S and a lower compression chamber 133S, which are lower cylinder chambers. The lower cylinder 121S has a lower suction hole 135S that communicates with the lower suction chamber 131S from its outer periphery. A lower compression section suction pipe 102S is connected to the lower suction hole 135S.
[0021] The upper end plate 160T has an upper discharge hole 190T that penetrates the upper end plate 160T and communicates with the upper compression chamber 133T. An upper discharge valve 200T, which is a reed valve that opens and closes the upper discharge hole 190T, and an upper discharge valve retainer 201T that regulates warping of the upper discharge valve 200T are fixed to the upper end plate 160T with upper rivets 202T. An upper end plate cover 170T that covers the upper discharge hole 190T is disposed above the upper end plate 160T, forming an upper end plate cover chamber 180T that is closed by the upper end plate 160T and the upper end plate cover 170T. The upper end plate cover 170T is fixed to the upper end plate 160T with a plurality of bolts 175 that also secure the upper end plate 160T to the upper cylinder 121T. The upper end plate cover 170T is provided with an upper end plate cover discharge hole 172T that connects the upper end plate cover chamber 180T with the inside of the main container 10. When the compression section 12 is provided inside the main container 10, the inner circumferential surface 10a of the main container 10 is shrink-fitted to the outer circumferential surface 182a of the upper end plate 160T and is joined to the main container 10 by a plurality of welded joints. The structure of the upper end plate 160T in this embodiment will be described in detail later.
[0022] The lower end plate 160S has a lower discharge hole 190S that penetrates the lower end plate 160S and communicates with the lower compression chamber 133S. A lower discharge valve 200S, which is a reed valve that opens and closes the lower discharge hole 190S, and a lower discharge valve retainer 201S that prevents the lower discharge valve 200S from warping are fixed to the lower end plate 160S with lower rivets 202S. A lower end plate cover 170S that covers the lower discharge hole 190S is disposed below the lower end plate 160S, forming a lower end plate cover chamber 180S that is closed by the lower end plate 160S and the lower end plate cover 170S (see FIG. 1 ). The lower end plate cover 170S is fixed to the lower end plate 160S with multiple bolts 175 that also secure the lower end plate 160S to the lower cylinder 121S.
[0023] In addition, the compression section 12 is provided with a refrigerant passage hole 136 (see Figure 2) that penetrates the lower end plate 160S, the lower cylinder 121S, the intermediate partition plate 140, the upper end plate 160T and the upper cylinder 121T and connects the lower end plate cover chamber 180S and the upper end plate cover chamber 180T.
[0024] The flow of refrigerant due to the rotation of the rotary shaft 15 will be described below. As the rotary shaft 15 rotates, the upper piston 125T fitted in the upper eccentric portion 152T of the rotary shaft 15 and the lower piston 125S fitted in the lower eccentric portion 152S revolve, causing the upper suction chamber 131T and the lower suction chamber 131S to expand in volume and draw in refrigerant. As a refrigerant intake path, low-pressure refrigerant from the refrigeration cycle is drawn into the accumulator 25 through the accumulator suction pipe 27, and only gaseous refrigerant is drawn into the upper gas-liquid separation pipe 31T and the lower gas-liquid separation pipe 31S. The gaseous refrigerant drawn into the upper gas-liquid separation pipe 31T passes through the upper connecting pipe 104T and the upper compression section suction pipe 102T and is drawn into the upper suction chamber 131T. Similarly, the gas refrigerant drawn into the lower gas-liquid separation pipe 31S passes through the lower connecting pipe 104S and the lower compression section suction pipe 102S and is drawn into the lower suction chamber 131S.
[0025] Next, we will explain the flow of refrigerant discharged by rotation of the rotary shaft 15. As the rotary shaft 15 rotates, the upper piston 125T fitted to the upper eccentric portion 152T of the rotary shaft 15 revolves, causing the upper compression chamber 133T to compress the refrigerant while reducing its volume. When the pressure of the compressed refrigerant becomes higher than the pressure in the upper end plate cover chamber 180T outside the upper discharge valve 200T, the upper discharge valve 200T opens and discharges the refrigerant from the upper compression chamber 133T into the upper end plate cover chamber 180T. The refrigerant discharged into the upper end plate cover chamber 180T is discharged into the main container 10 through the upper end plate cover discharge hole 172T provided in the upper end plate cover 170T.
[0026] Furthermore, as the rotary shaft 15 rotates, the lower piston 125S fitted into the lower eccentric portion 152S of the rotary shaft 15 revolves, compressing the refrigerant while reducing the volume of the lower compression chamber 133S, and when the pressure of the compressed refrigerant becomes higher than the pressure in the lower end plate cover chamber 180S outside the lower discharge valve 200S, the lower discharge valve 200S opens and discharges the refrigerant from the lower compression chamber 133S to the lower end plate cover chamber 180S. The refrigerant discharged into the lower end plate cover chamber 180S passes through the refrigerant passage hole 136 and the upper end plate cover chamber 180T and is discharged into the main container 10 from the upper end plate cover discharge hole 172T provided in the upper end plate cover 170T.
[0027] The refrigerant discharged into the main container 10 is guided above the motor 11 through a notch (not shown) on the outer periphery of the stator 111 that connects the top and bottom, or a gap (not shown) in the winding section of the stator 111, or a gap 115 (see Figure 1) between the stator 111 and the rotor 112, and is discharged from a discharge pipe 107 located at the top of the main container 10.
[0028] Next, the flow of lubricating oil 18 will be described. Lubricating oil 18 sealed in the lower part of main container 10 is supplied to compression section 12 through the interior of rotating shaft 15 (not shown) by the centrifugal force of rotating shaft 15. Lubricating oil 18 supplied to compression section 12 is entrained in the refrigerant and atomized, and then discharged into main container 10 together with the refrigerant. The mist of lubricating oil 18 discharged into main container 10 is separated from the refrigerant by centrifugal force caused by the rotational force of motor 11, and returns to the bottom of main container 10 as oil droplets. However, some of the lubricating oil 18 is not separated and is discharged into the refrigeration cycle together with the refrigerant. Lubricating oil 18 discharged into the refrigeration cycle circulates through the refrigeration cycle and returns to accumulator 25, where it is separated and accumulates in the lower part of accumulator 25. The lubricating oil 18 accumulated in the lower part of accumulator 25 is drawn into upper suction chamber 131T and lower suction chamber 131S together with the suctioned refrigerant.
[0029] (Characteristic Configuration of Compressor 1) Next, the characteristic configuration of the vane of the first embodiment will be described. FIG. 3 is a perspective view showing the vane of the first embodiment. Because the upper vane 127T and the lower vane 127S (hereinafter also referred to as vane 127) have the same structure, the following description will focus on the upper vane 127T, and the description of the lower vane 127S will be omitted. The upper vane 127T has a tip surface 129a that slides against the outer circumferential surface of the upper piston 125T, and a first side surface 129b and a second side surface 129c that slide against the inner surface of the upper vane groove 128T. The upper vane 127T also has a first end surface 129d that slides against the end surface of the upper end plate 160T, a second end surface 129e that slides against the end surface of the intermediate partition plate 140 serving as an end plate, and a back surface 129f that is pressed by the upper spring 126T. Regarding lower vane 127S, lower vane 127S has a first end face 129d that slides against the end face of intermediate partition plate 140 serving as an end plate, and a second end face 129e that slides against the end face of lower end plate 160S. First side face 129b and second side face 129c, first end face 129d and second end face 129e are each formed in a flat plate shape.
[0030] The tip end surface 129a of the upper vane 127T is formed in an arc shape when viewed from a direction perpendicular to the first end surface 129d and the second end surface 129e. An engagement portion 138, which engages with an end of the upper spring 126T, is formed on the back surface 129f of the upper vane 127T by cutting out a part of the flat back surface 129f.
[0031] The upper vane 127T includes a base material 210 and a hard coating 220. The base material 210 has a base material layer 211 (described later) formed of a material with a chromium (Cr) content exceeding 4.5 wt%. Examples of such materials include SUS440C (a type of martensitic stainless steel) with a chromium (Cr) content of approximately 16 wt% to 18 wt%, SKD61 (a type of die steel) with a chromium (Cr) content of approximately 4.8 wt% to 5.5 wt%, and SKD11 (a type of die steel) with a chromium (Cr) content of approximately 11.0 wt% to 13.0 wt%. In this way, the base material layer 211 of the base material 210 is formed of a material with a chromium (Cr) content exceeding 4.5 wt%, thereby ensuring appropriate wear resistance and seizure resistance for the upper vane 127T. Furthermore, when the base material layer 211 of the base material 210 of the upper vane 127T is formed from stainless steel with a chromium (Cr) content exceeding 10 wt %, the wear resistance and seizure resistance of the first side surface 129b and the second side surface 129c, which have a particularly large sliding area, can be sufficiently ensured.
[0032] Fig. 4 is a cross-sectional view showing the hard coating 220 of the vane 127 of Example 1. Fig. 4 shows a cross-section perpendicular to the first end face 129d and the second end face 129e of the vane 127. Fig. 5 is an enlarged cross-sectional view showing the tip of the vane 127 of Example 1. Fig. 5 shows a cross-section perpendicular to the first side face 129b and the second side face 129c of the vane 127.
[0033] 4, a hard coating 220 is formed on the tip end surface 129a of the upper vane 127T. A nitride diffusion layer 212 is formed on the entire outer peripheral surface of the base material 210 so as to cover the base material layer 211, and a dense layer 213 is formed on the nitride diffusion layer 212.
[0034] As shown in Fig. 5, a hard coating 220 is formed over the entire tip end surface 129a of the upper vane 127T. The hard coating 220 is formed on the surface side of the dense layer 213 of the base material 210 and is in close contact with the dense layer 213. The hard coating 220 is made of, for example, dichromium nitride (CrN) having a Vickers hardness of 1500 HV or more. 2The upper vane 127T is formed of a hard coating 220 on the tip end surface 129a thereof, thereby ensuring appropriate wear resistance of the tip end surface 129a.
[0035] (Method of Manufacturing Vane) The method of manufacturing the vane of Example 1 is a method of manufacturing the vane 127 of Example 1 configured as described above. Figure 6 is a schematic diagram for explaining the method of manufacturing the vane of Example 1. Figure 6 shows the process by which the properties of the vane 127 change according to the method of manufacturing the vane of Example 1.
[0036] The entire base material 210 of the vane 127 before nitriding is formed from a material with a chromium (Cr) content of more than 4.5 wt %. In the embodiment, a region of the base material 210 having the same composition as the base material 210 before nitriding is referred to as a base material layer 211. The high chromium (Cr) content in the base material layer 211 of the base material 210 ensures appropriate wear resistance and seizure resistance of the vane 127. In the vane 127 of the first embodiment, for example, the base material layer 211 of the base material 210 is formed from martensitic stainless steel with a chromium (Cr) content of approximately 16 wt % to 18 wt %. The vane 127 has a base material layer 211 of a base material 210 formed from stainless steel with a chromium (Cr) content exceeding 10 wt %, thereby ensuring sufficient wear resistance and seizure resistance, particularly for the first side surface 129b and the second side surface 129c, which have a large sliding area.
[0037] After the base material 210 is formed, the base material 210 is quenched (a heat treatment in which a metal is heated to an austenitic structure and then rapidly cooled to obtain a martensite structure). This quenching improves the wear resistance and mechanical strength of the base material 210. After quenching the base material 210, the base material 210 is tempered (a heat treatment in which a metal whose structure has become unstable due to quenching or the like is maintained at an appropriate temperature to stabilize the metal structure). This tempering improves the toughness of the base material 210.
[0038] After the base material 210 is tempered, the base material 210 is subjected to a nitriding treatment (step S1). Examples of nitriding treatment include gas nitriding, gas soft nitriding, and ion nitriding. In the nitriding treatment, nitrogen atoms N penetrate and diffuse from the surface of the base material 210 to the interior, and a nitride layer 214 is formed on the surface of the base material 210 after the treatment of step S1 has been performed. Therefore, the nitride layer 214 is formed so as to surround the base material layer 211. Here, the nitride layer 214 refers to a layer formed by changing the structure of the base material layer 211 through the nitriding treatment. Note that a portion of the base material 210 formed with the same composition as the base material layer 211 of the base material 210 immediately before the nitriding treatment will continue to be referred to as the base material layer 211 even after the nitriding treatment.
[0039] FIG. 7 is an enlarged cross-sectional view showing the surface of the base material 210 immediately after nitriding. In this embodiment, the nitride layer 214 is formed from a nitride diffusion layer 212 and a nitride compound layer 216 (white layer). The nitride diffusion layer 212 is formed on the outer surface side of the base material layer 211. The nitride diffusion layer 212 is formed from an α (alpha) phase with a body-centered cubic crystal structure. The nitride diffusion layer 212 is formed from a material in which nitrogen atoms N are solid-dissolved in the metal forming the base material layer 211, or a material in which chromium (Cr) nitrides are dispersed and precipitated in the material in which nitrogen atoms N are solid-dissolved. Furthermore, nitrogen atoms N are diffused into the nitride diffusion layer 212 so as to form a concentration gradient in which the concentration of nitrogen atoms N decreases toward the base material layer 215.
[0040] The nitride compound layer 216 (white layer) is formed from a material with a higher nitrogen concentration than the material from which the nitride diffusion layer 212 is formed, and is formed from a material that is harder and more brittle than the nitride diffusion layer 212. The nitride compound layer 216 is formed from a dense layer 213 and a porous layer 217. The dense layer 213 is formed on the outer surface side of the nitride diffusion layer 212. The dense layer 213 is made of iron nitride Fe 4 The porous layer 217 is formed on the outer surface side of the dense layer 213 and on the outermost surface of the nitrided layer 214 of the nitrided base material 210. The porous layer 217 is composed mainly of iron nitride (Fe). 2 N, Fe 3The base material 210 is composed mainly of N and is formed from the ε (epsilon) phase with a close-packed hexagonal structure. Therefore, immediately after the nitriding treatment, the surface of the base material 210 has a porous layer 217, a dense layer 213, a nitride diffusion layer 212, and a base material layer 211 arranged in this order from the outside.
[0041] After nitriding the base material 210, the surface of the base material 210 is ground (step S2). In this step, the surface layers of the nitride layer 216 formed on the tip surface 129a, the first side surface 129b, the second side surface 129c, the first end surface 129d, and the second end surface 129e are ground. This grinds away the surface layer, which has small bulges and small depressions that have occurred on the surface of the base material 210 due to the nitriding process, and flattens the first side surface 129b, the second side surface 129c, the first end surface 129d, and the second end surface 129e, thereby ensuring the dimensional accuracy and surface accuracy (flatness) of the vane 127 that slides against the inner surface of the upper vane groove 128T (lower vane groove 128S), the end surface of the upper end plate 160T (lower end plate 160S), and the intermediate partition plate 140. In this embodiment, at least the porous layer 217 of the nitride layer 216 (white layer) is removed so that the dense layer 213 is exposed on the surface of the tip end face 129a of the base material 210 after the processing of step S2 is performed.
[0042] After the surface of the base material 210 is scraped, a hard film 220 is formed on the tip end surface 129a of the base material 210 by a sputtering method (step S3). The hard film 220 is made of, for example, chromium nitride (CrN) having a Vickers hardness of 1500 HV or more. 2 This improves the wear resistance of the tip end surface 129a of the vane 127 after the process in step S3. In this embodiment, the hard coating 220 is formed so as to adhere closely to the dense layer 213 of the tip end surface 29a. The hard coating 220 formed by the sputtering method is made of dichromium nitride (Cr 2 The material is not limited to chromium nitride (N), but may be chromium nitride (CrN), for example.
[0043] As shown in Fig. 8, the hard coating 220 is formed on the front end surface 129a of the base material 210 by a sputtering method using a film forming apparatus 230. Fig. 8 is a cross-sectional view showing the film forming apparatus 230 that forms the hard coating 220 on the front end surface 129a of the base material 210 by a sputtering method. The film forming apparatus 230 includes a furnace 231 and a target 232. A processing chamber 233 is formed inside the furnace 231. The target 232 is made of metallic chromium Cr.
[0044] 9 is a schematic diagram illustrating an example of the process of forming the hard coating 220 in Example 1. In the process of forming the hard coating 220 (step S3), a plurality of base materials 210 are arranged in a processing chamber 233 provided in a film-forming apparatus 230. The plurality of base materials 210 are arranged so that the side surfaces 129 b, 129 c of adjacent base materials 210, i.e., the opposing first side surfaces 129 b and second side surfaces 129 c, are in contact with each other, and so that the end surfaces 129 d, 129 e of adjacent base materials 210, i.e., the opposing first end surfaces 129 d and second end surfaces 129 e, are in contact with each other.
[0045] After the plurality of base materials 210 are arranged in the processing chamber 233, the film forming apparatus 230 reduces the pressure inside the processing chamber 233 and fills it with an inert gas (for example, argon Ar) and nitrogen gas N 2 The film forming apparatus 230 is configured to introduce an inert gas and nitrogen gas N 2 8, a high voltage is applied to the target 232 and the plurality of base materials 210 so that the target 232 is negatively charged and the plurality of base materials 210 is positively charged. By applying a high voltage between the target 232 and the plurality of base materials 210, plasma is generated in the processing chamber 233, the inert gas becomes ions 234, and the ions 234 collide with the target 232. When the ions 234 collide with the target 232, a sputtering phenomenon occurs in which chromium atoms Cr that form the target 232 are released from the target 232.
[0046] The chromium atoms Cr emitted from the target 232 are attached to the tip surfaces 129a of the plurality of base materials 210 together with the nitrogen atoms N. As a result, the tip surfaces 129a of the plurality of base materials 210 are covered with dichromium nitride (Cr 2 9 ). In other words, the film forming device 230 collectively forms the hard coating 220 on each of the tip surfaces 129 a of the plurality of base materials 210 arranged as shown in FIG. 9 . This allows the number of base materials 210 on which the hard coating 220 is formed in one forming process to be increased, thereby reducing the manufacturing cost of the vane 127.
[0047] Furthermore, by arranging adjacent base materials 210 so that the side surfaces 129b, 129c and the end surfaces 129d, 129e are in contact with each other, the side surfaces 129b, 129c and the end surfaces 129d, 129e can be masked to prevent the hard coating 220 from being formed on the side surfaces 129b, 129c and the end surfaces 129d, 129e. By using other vanes 127 as masking members for coating the vanes 127 in this way, it is not necessary to provide a separate process for masking the surfaces of the base materials 210 on which the hard coating 220 is not to be formed, and the masking process can be reduced. By eliminating the masking process, the vane manufacturing method can reduce the manufacturing costs of the vanes 127.
[0048] The adhesion of the hard coating 220 to the dense layer 213 is better than the adhesion of the hard coating 220 to the porous layer 217. Therefore, the vane 127 manufactured so that the hard coating 220 is in close contact with the dense layer 213 can more strongly adhere the hard coating 220 to the base material 210 than other vanes in which the hard coating 220 is in close contact with the base material 210 via the porous layer 217, and can prevent the hard coating 220 from peeling off from the tip end surface 127 a.
[0049] Furthermore, the porous layer 217 has the characteristics of being hard but brittle. Therefore, the vane 127 of Example 1, in which the porous layer 217 is removed to expose the dense layer 213 on the surface of the base material 210 and the hard coating 220 is then formed so as to adhere to the dense layer 213, can prevent abnormal wear caused by the porous layer 217 coming off during sliding at high surface pressure, compared to other vanes in which the hard coating 220 and the base material 210 are in close contact with each other via the porous layer 217.
[0050] When the hard film 220 is formed by sputtering using metallic chromium Cr as the target 232, it may be difficult to form the hard film 220 of chromium nitride (CrN) depending on the film forming device 240. 2 The hard film 220 of dichromium nitride (Cr) can be easily formed stably regardless of the film forming device 240. 2 By using the above-mentioned CrN, the hard coating 220 can be stably formed even when a sputtering method is used.
[0051] The vane of the comparative example has a hard coating 220 formed by an arc ion plating method, which is different from sputtering, and other portions are formed in the same manner as the vane 127 of the first embodiment described above. Figure 10 is a cross-sectional view showing another film formation apparatus 230 that forms the hard coating 220 on the tip surface 129a of the vane 127 of the comparative example by arc ion plating. The film formation apparatus 240 includes a furnace 241 and a target 232. A processing chamber 243 is formed inside the furnace 241. The target 242 is made of metallic chromium Cr.
[0052] After a plurality of base materials 210 are arranged in the processing chamber 243, the film forming apparatus 240 reduces the pressure inside the processing chamber 243 and introduces nitrogen gas N2 into the processing chamber 243. After the nitrogen gas N2 is introduced into the processing chamber 243, the film forming apparatus 240 generates an arc in the processing chamber 243 and heats the target 242. The metallic chromium Cr that forms the target 242 evaporates when the target 242 is heated. At this time, the target 242 (metallic chromium Cr) melted by the heating may not be ionized, and droplets measuring several tens of microns may be generated in the processing chamber 243. The droplets may be, for example, chromium nitride CrN or dichromium nitride Cr 2 The film forming device 240 applies a voltage so that the evaporated metallic chromium Cr is positively charged and the plurality of base materials 210 is negatively charged. By applying the voltage, the evaporated metallic chromium Cr adheres to the tip surfaces 129a of the plurality of base materials 210 together with nitrogen atoms N. As a result, the tip surfaces 129a of the plurality of base materials 210 are coated with dichromium nitride Cr. 2 A hard coating 220 made of N is formed.
[0053] At this time, the droplets generated in the processing chamber 243 may not ionize but may adhere to the tip end surface 129a of the base material 210 together with the evaporated metallic chromium Cr and be incorporated into the hard coating 220. Therefore, as shown in FIG. 11 , protrusions 245 formed from the droplets may be formed on the hard coating 220 of the vane of the comparative example. FIG. 11 is a perspective view showing the surface of the hard coating 220 of the vane of the comparative example. When the protrusions 245 are formed on the tip end surface 129a of the vane of the comparative example, the vane of the comparative example is highly aggressive to the sliding counterpart that slides against the tip end surface 129a of the vane of the comparative example. Therefore, in a compressor equipped with the vane of the comparative example, the protrusions 245 come into contact with the upper piston 125T or the lower piston 125S, which is prone to wear of the upper piston 125T or the lower piston 125S. Therefore, the amount of wear on the surface of the upper piston 125T or the lower piston 125S caused by the vane of the comparative example is greater than the amount of wear on the surface of the upper piston 125T or the lower piston 125S caused by the vane 127 of the first embodiment described above.
[0054] The vane 127 of Example 1, in which the hard coating 220 is formed by sputtering, can prevent droplets from being generated in the processing chamber 243 and can prevent the formation of protrusions 245 on the tip end surface 129 a. Therefore, the vane 127 of Example 1 can reduce wear on the surface of the upper piston 125T or the lower piston 125S compared to the vane of the comparative example.
[0055] (Effect of vane 127 of Example 1) The vane 127 of Example 1 is used in a compressor 1 that includes an upper cylinder 121T (lower cylinder 121S), an upper piston 125T (lower piston 125S) that revolves along the inner surface of the upper cylinder 121T (lower cylinder 121S), and an upper end plate 160T (lower end plate 160S, intermediate partition plate 140) that closes the end of the upper cylinder 121T (lower cylinder 121S), and divides the upper cylinder chamber (lower cylinder chamber) surrounded by the upper cylinder 121T (lower cylinder 121S), the upper piston 125T (lower piston 125S), and the upper end plate 160T (lower end plate 160S, intermediate partition plate 140) into an upper suction chamber 131T (lower suction chamber 131S) and an upper compression chamber 133T (lower compression chamber 133S). The vane 127 includes a nitrided base material 210 and a hard coating 220 that coats a tip end surface 129a of the base material 210. The hard coating 220 is formed by sputtering. This prevents droplet-derived protrusions 245 from being formed on the tip end surface 129a of the vane 127, which would otherwise be formed on a hard coating formed by arc ion plating. Therefore, the vane 127 of Example 1 can reduce wear of the upper piston 125T (lower piston 125S) that contacts the tip end surface 129a while ensuring the hardness of the tip end surface 129a with the hard coating 220.
[0056] The hard coating 220 of the vane 127 of Example 1 has a Vickers hardness of 1500 HV or more. This ensures that the vane 127 has adequate wear resistance on the tip end surface 129a. For example, the hard coating 220 is made of chromium nitride (CrN). 2The vane 127 is formed from N. This allows the vane 127 to appropriately ensure the wear resistance of the tip end surface 129a against the upper piston 125T (lower piston 125S).
[0057] Furthermore, the base material 210 of the vane 127 of Example 1 is formed from a material with a chromium content of more than 4.5 wt %, for example, stainless steel with a chromium content of 10.5 wt % or more. For example, the base material 210 of the vane 127 of Example 1 is formed from martensitic stainless steel with a chromium (Cr) content of approximately 16 wt % to 18 wt %. In this way, the high chromium (Cr) content in the base material layer 211 of the base material 210 of the vane 127 ensures sufficient wear resistance and seizure resistance, particularly for the first side surface 129 b, the second side surface 129 c, the first end surface 129 d, and the second end surface 129 e, which have large sliding areas.
[0058] The base material 210 of the vane 127 of Example 1 includes a base material layer 211, a nitride diffusion layer 212 formed outside the base material layer 211, and an iron nitride (Fe) layer formed outside the nitride diffusion layer 212. 4 A dense layer 213 made of a gamma prime phase containing N as a main component is formed. At this time, a hard coating 220 is formed on the surface of the dense layer 213. Such a vane 127 can make the hard coating 220 adhere more strongly to the base material 210, and can prevent the hard coating 220 from peeling off from the tip end surface 127a.
[0059] The base material 210 of the vane 127 of the first embodiment further includes a first side surface 129b and a second side surface 129c that slide on the upper cylinder 121T (lower cylinder 121S), and a first end surface 129d (second end surface 129e) that slides on the upper end plate 160T (lower end plate 160S, intermediate partition plate 140). The first side surface 129b, the second side surface 129c, and the first end surface 129d (second end surface 129e) of the base material 210 are made of iron nitride Fe 4A dense layer 213 made of a gamma prime phase containing N as a main component is exposed on the outer surface. Such vane 127 can ensure sufficient wear resistance and seizure resistance for the sliding surfaces other than tip end surface 129a (first side surface 129b, second side surface 129c, first end surface 129d, and second end surface 129e).
[0060] The manufacturing method for the vane of Example 1 is a manufacturing method used when manufacturing the vane 127 of Example 1, and includes a step of nitriding the base material 210 (step S1) and a step of forming the hard coating 220 by a sputtering method after nitriding the base material 210 (step S3). This manufacturing method for the vane can prevent the formation of the droplet-derived protrusions 245 on the tip end surface 129a. Therefore, the vane 127 manufactured by this manufacturing method can reduce wear of the upper piston 125T (lower piston 125S) that comes into contact with the tip end surface 129a.
[0061] In the manufacturing method of the vane of the first embodiment, iron nitride Fe is added to the base material 210 before the step of forming the hard coating 220 on the tip end surface 129a of the base material 210 (step S3). 2 N, Fe 3 By removing the porous layer 217 made of the epsilon phase containing N as the main component, iron nitride Fe is formed on the tip surface 129a of the base material 210. 4 The method further includes a step (step S2) of exposing dense layer 213 made of a gamma prime phase containing N as a main component. This vane manufacturing method can appropriately manufacture vane 127, which can form hard coating 220 on the surface of dense layer 213 and prevent hard coating 220 from peeling off tip end surface 129 a.
[0062] In the manufacturing method of the vane of Example 1, iron nitride Fe 4The method further includes a step (step S2) of exposing dense layer 213 made of a gamma prime phase containing N as a main component on the outer surfaces of first side surface 129 b, second side surface 129 c, first end face 129 d, and second end face 129 e of base material 210. This vane manufacturing method can appropriately produce vane 127 that has sufficient wear resistance and seizure resistance also for first side surface 129 b, second side surface 129 c, first end face 129 d, and second end face 129 e, which are sliding surfaces other than tip end surface 129 a.
[0063] The base material 210 further includes a first side surface 129b and a second side surface 129c that slide against the upper cylinder 121T (lower cylinder 121S), and a first end surface 129d (second end surface 129e) that slides against the upper end plate 160T (lower end plate 160S, intermediate partition plate 140). In the vane manufacturing method of Example 1, in the process of forming the hard coating 220 on the base material 210 (step S3), multiple base materials 210 are arranged so that the first side surfaces 129b and the second side surfaces 129c or the first end surfaces 129d (second end surfaces 129e) of adjacent base materials 210 are in contact with each other, and the hard coating 220 is formed on each tip surface 129a of the multiple base materials 210 at one time. This vane manufacturing method reduces the manufacturing cost of the vane 127.
[0064] As shown in Figures 12 and 13, the vane of Example 2 is the same as the vane 127 of Example 1 described above, except that the dense layer 213 of the vane 127 of Example 1 described above is omitted. Figure 12 is a cross-sectional view showing the vane of Example 2. Figure 13 is a schematic diagram for explaining the manufacturing method of the vane of Example 2. Figure 13 shows the process by which the properties of the vane 127 change due to the manufacturing method of the vane of Example 2.
[0065] The vane of Example 2, like the vane 127 of Example 1, has a hard coating 220 formed over the entire tip end surface 129a. The hard coating 220 is formed on the surface of the nitride diffusion layer 212 of the base material 210 and is in close contact with the nitride diffusion layer 212. The vane of Example 2 differs from the vane of Example 1 in that the hard coating 220 is in close contact with the nitride diffusion layer 212 as a result of the removal of not only the porous layer 217 but also the dense layer 213 in the process of scraping the surface of the base material 210, which will be described later.
[0066] The vane manufacturing method of Example 2 is a method for manufacturing the vane 127 of Example 2. As shown in FIG. 13 , steps S2 and S3 of the manufacturing method of the vane of Example 1 described above are replaced with steps S4 and S5, respectively, but the remaining steps are the same as those of the manufacturing method of the vane of Example 1 described above. FIG. 13 is a schematic diagram for explaining an example of the process for forming the hard coating 220 in Example 2. Step S1 of the manufacturing method of the vane of Example 2 is the same as step S1 of the manufacturing method of the vane of Example 1 described above. After the base material 210 is nitrided in step S1, the surface of the base material 210 is scraped, and the dense layer 213 and the porous layer 217 are removed so that the nitride diffusion layer 212 is exposed on the surface of the base material 210 (step S4). That is, in step S4, the entire nitride compound layer 216 (white layer) of the nitride layer 214 is removed. After the surface of the base material 210 is scraped in step S4, a hard coating 220 is formed on the nitride diffusion layer 212 on the tip end surface 129a of the base material 210 (step S5). According to this vane manufacturing method, the vane 127 of Example 2 is appropriately manufactured so that the hard coating 220 formed in step S5 is formed on the surface of the nitride diffusion layer 212 of the base material 210 and adheres closely to the nitride diffusion layer 212.
[0067] The adhesion of the hard coating 220 to the nitride diffusion layer 212 is roughly equivalent to the adhesion of the hard coating 220 to the dense layer 213, and is better than the adhesion of the hard coating 220 to the porous layer 217. Therefore, like the vane 127 of the first embodiment, the vane of the second embodiment can more strongly adhere the hard coating 220 to the base material 210, and can prevent the hard coating 220 from peeling off from the tip end surface 127 a, compared to other vanes in which the hard coating 220 and the base material 210 are in close contact with each other via the porous layer 217.
[0068] In the vane of Example 2, the nitride diffusion layer 212 is exposed on the surface where the hard coating 220 is not formed, and the first side surface 129b, the second side surface 129c, the first end surface 129d, and the second end surface 129e are formed from the nitride diffusion layer 212. Like the dense layer 213, the nitride diffusion layer 212 has better wear resistance and seizure resistance than the base material layer 211. Therefore, like the vane 127 of Example 1 described above, the vane of Example 2 can ensure wear resistance and seizure resistance even on the surface where the hard coating 220 is not formed.
[0069] In the vane manufacturing method of Example 2 described above, the entire surface of the base material 210 is scraped in step S4 so as to remove both the dense layer 213 and the porous layer 217. However, the surface of the base material 210 may also be scraped so that the dense layer 213 remains on a surface (side surface or end surface) other than the tip end surface 129a. In a vane manufactured by such a manufacturing method, as in the vane of Example 2 described above, the hard coating 220 is in close contact with the nitride diffusion layer 212 on the tip end surface 129a. This ensures the hardness of the tip end surface 129a, which requires particularly high wear resistance, while preventing the hard coating 220 from peeling off from the tip end surface 129a. Furthermore, the dense layer 213 ensures the wear resistance and seizure resistance of the sliding surfaces (side surface and end surface) other than the tip end surface 129a, where the hard coating 220 is not formed.
[0070] In the vane manufacturing methods of the previously described embodiments, the entire surface of the base material 210 is removed in step S2 in Example 1 and in step S4 in Example 2 to remove the porous layer 217. However, the base material may be removed so that the porous layer 217 remains on a surface (side or end surface) other than the tip end surface 129a. In vanes manufactured by such a manufacturing method, as in the vanes of the previously described embodiments, the hard coating 220 is in close contact with the dense layer 213 or the nitride diffusion layer 212 on the tip end surface 129a, which requires particularly high wear resistance, and this prevents the hard coating 220 from peeling off from the tip end surface 129a. Furthermore, the porous layer 217 (nitride layer 216) ensures the wear resistance and seizure resistance of the surface on which the hard coating 220 is not formed.
[0071] In the vane manufacturing method of the above-described embodiment, the hard coating 220 is formed on the tip surfaces 129a of the plurality of base materials 210 with the side surfaces and end surfaces in close contact with each other, but the hard coating 220 may also be formed on the tip surfaces 129a of the plurality of base materials 210 with the side surfaces and end surfaces not in close contact with each other. In this case, surfaces (side surfaces and end surfaces) of the plurality of base materials 210 different from the tip surfaces 129a may be masked to prevent the hard coating 220 from being formed thereon.
[0072] In the vanes of the previously described embodiments, the hard coating 220 is formed on the surface of the dense layer 213 or the nitride diffusion layer 212, but the hard coating 220 may be formed on the surface of the base material layer 211 in close contact with the base material layer 211. In such vanes, the hard coating 220 is formed by sputtering, which prevents the formation of protrusions 245 on the tip end surface 129a, as in the vanes of the previously described embodiments, and reduces wear on the surface of the upper piston 125T or the lower piston 125S.
[0073] In the above-described embodiment, a two-cylinder rotary compressor having two cylinders 121, an upper cylinder 121T and a lower cylinder 121S, was exemplified as the compressor 1, but it may also be a one-cylinder rotary compressor having only one cylinder 121.
[0074] Although the embodiments have been described above, the embodiments are not limited to the above content. Furthermore, the above-described components include those that can be easily imagined by a person skilled in the art, those that are substantially the same, and those that are within the scope of so-called equivalents. Furthermore, the above-described components can be combined as appropriate. Furthermore, at least one of various omissions, substitutions, and modifications of the components can be made within the scope that does not deviate from the gist of the embodiments.
[0075] DESCRIPTION OF SYMBOLS 1 Compressor 121T Upper cylinder (cylinder) 121S Lower cylinder (cylinder) 125T Upper piston (piston) 125S Lower piston (piston) 127 Vane 127T Upper vane (vane) 127S Lower vane (vane) 129a Tip surface 129b First side surface 129c Second side surface 129d First end surface 129e Second end surface 160T Upper end plate (end plate) 160S Lower end plate (end plate) 210 Base material 211 Base material layer 212 Nitrided diffusion layer 213 Dense layer 214 Nitrided layer 216 Nitrided compound layer 217 Porous layer 220 Hard coating
Claims
1. A vane used in a compressor comprising: a cylinder; a piston that revolves along the inner circumferential surface of the cylinder; and an end plate that closes an end of the cylinder, the vane dividing a cylinder chamber surrounded by the cylinder, the piston, and the end plate into a suction chamber and a compression chamber, the vane comprising: a nitrided base material; and a hard coating that covers a tip end surface of the base material, the hard coating being formed by a sputtering method.
2. The vane according to claim 1, wherein the hard coating has a Vickers hardness of 1500 HV or more.
3. The hard coating is made of Cr 2 The vane of claim 1 formed from N.
4. The vane according to claim 1, wherein the base material is formed from a material having a chromium content of more than 4.5 wt %.
5. The vane according to claim 4, wherein the base material is formed from stainless steel having a chromium content of 10.5 wt % or more.
6. The vane according to claim 5, wherein the base material is formed from martensitic stainless steel.
7. The vane according to claim 1, wherein the base material is provided with a base material layer and a nitride diffusion layer formed outside the base material layer, and the hard coating is formed on a surface of the nitride diffusion layer.
8. The base material includes a base layer, a nitride diffusion layer formed outside the base layer, and an Fe diffusion layer formed outside the nitride diffusion layer. 4 The vane according to claim 1 , wherein a dense layer made of a gamma prime phase containing N as a main component is formed, and the hard coating is formed on a surface of the dense layer.
9. The base material further includes a side surface that slides against the cylinder and an end surface that slides against the end plate, and the side surface and the end surface of the base material are provided with the nitride diffusion layer or the Fe 4 The dense layer is made of a gamma prime phase mainly composed of N, or 2 N, Fe 3 The vane according to claim 8 , wherein any one of the porous layers containing N as a main component is exposed.
10. A compressor comprising: a cylinder; a piston which revolves along the inner circumferential surface of the cylinder; an end plate which closes the end of the cylinder; and a vane which divides a cylinder chamber enclosed by the cylinder, the piston and the end plate into a suction chamber and a compression chamber, wherein the vane has a nitrided base material and a hard coating which covers a tip surface of the base material, the hard coating being formed by a sputtering method.
11. A method for manufacturing a vane used in a compressor comprising: a cylinder; a piston that revolves along the inner surface of the cylinder; an end plate that closes the end of the cylinder; and a vane that divides a cylinder chamber surrounded by the cylinder, the piston, and the end plate into a suction chamber and a compression chamber, the vane having a base material and a hard coating that covers a tip surface of the base material, the method comprising the steps of: nitriding the base material; and forming the hard coating by a sputtering method after nitriding the base material.
12. Prior to the step of forming the hard coating, the base material is subjected to a nitriding treatment to form a nitride compound layer on the base material, and at least Fe 2 N, Fe 3 By removing the porous layer made of the epsilon phase mainly composed of N, a nitride diffusion layer or an Fe diffusion layer is formed on the tip surface of the base material. 4 12. The method for manufacturing a vane according to claim 11, further comprising a step of exposing any one of layers of a dense layer made of a gamma prime phase containing N as a main component, wherein in the step of forming the hard coating on the tip end surface of the base material, the hard coating is formed on the tip end surface of the base material from which the nitride diffusion layer or the dense layer is exposed, and the base material of the vane is formed from a material having a chromium content of more than 4.5 wt%.
13. The base material has a side surface that slides against the vane groove formed in the cylinder and an end surface that slides against the end plate, and the nitride diffusion layer or the Fe 4 The dense layer is made of a gamma prime phase mainly composed of N, or 2 N, Fe 3 The method for manufacturing a vane according to claim 12, further comprising the step of exposing any one of the porous layers made of an epsilon phase containing N as a main component.
14. A method for manufacturing a vane as described in claim 11, further comprising the base material, a side surface that slides against the cylinder, and an end surface that slides against the end plate, wherein in the step of forming the hard coating on the base material, the multiple base materials are arranged so that the side surfaces or end surfaces of two adjacent base materials among the multiple base materials are in contact with each other, and the hard coating is formed simultaneously on each tip surface of the multiple base materials.
Citation Information
Patent Citations
Rotary type fluid compressor
JP1993078792A
Vane for rotary compressor
JP2000136784A
Nitrided vane for rotary compressor and its manufacturing method
JP2005016386A
Vane for refrigerant compressors, method of manufacturing the same and refrigerant compressor
JP2005048687A
Coating film deposition method, and coating base material
JP2007191751A
Cited By
Method of manufacturing vanes
JP7852695B1
Method for manufacturing vane
WO2026133746A1