Fluorescent body powder, fluorescent body resin composition, fluorescent body, light-emitting element, and light-emitting device
The development of a phosphor powder with enhanced blue light absorption addresses the limitations of conventional materials, achieving superior color purity and design flexibility for light-emitting devices by optimizing fluorescence intensity ratios and compositions.
Patent Information
- Application Number
- PCT/JP2024/003761
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-02-05
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional fluorescent materials for LEDs have insufficient blue light absorption rates, leading to contamination of unwanted luminescent colors and difficulties in achieving desired color tones in light-emitting devices.
A phosphor powder with a high absorption rate for blue light is developed, characterized by specific fluorescence intensity ratios and compositions, including a host compound and luminescence center elements, which enhances the absorption of blue light and suppresses its transmission.
The phosphor powder achieves a high absorption rate for blue light, resulting in improved color purity and design flexibility for light-emitting elements, enabling the production of high-quality images with enhanced luminescent colors in applications like micro LED displays.
Smart Images

Figure JP2024003761_03102024_PF_FP_ABST
Abstract
Description
Phosphor powder, phosphor resin composition, phosphor, light-emitting element, and light-emitting device
[0001] The present invention relates to a phosphor powder, a phosphor resin composition, a phosphor, a light-emitting element, and a light-emitting device.
[0002] Light-emitting devices that use light-emitting diodes (LEDs) that emit near-ultraviolet light or blue light as a light source (excitation source) and combine this with a phosphor are widely used in various light-emitting devices such as lighting, backlights for mobile terminals, and displays.
[0003] In this light-emitting device, the phosphor absorbs the light emitted by the LED (radiated light) and emits light of a different wavelength from the absorbed light. Therefore, it is possible to obtain light of a different color tone from the LED-radiated light. For example, by combining a blue-emitting LED (blue LED) with a green phosphor and / or a red phosphor, green light, red light, or white light can be obtained.
[0004] As a document disclosing the use of phosphors for LEDs, for example, Patent Document 1 discloses a white light-emitting device that includes a light-emitting diode that emits blue light, a thiogallate-based green phosphor that emits green light, and an alkaline earth metal sulfide-based red phosphor that emits red light, and that emits white light by mixing the green light and the red light with a part of the blue light (claim 3 of Patent Document 1).It also describes that the white light-emitting device is used as a backlight source for lighting, laptop computers, etc. (paragraph
[0002] of Patent Document 1).
[0005] Turning to displays, another application of phosphors, mini LED displays and micro LED displays have been attracting attention in recent years as display technology has advanced. Micro LED displays use independent LEDs for each of the R (red), G (green), and B (blue) subpixels, offering advantages over LCD panels, including the ability to achieve higher brightness, higher contrast ratios, faster response times, and lower power consumption. Furthermore, compared to organic electroluminescence (EL) displays, they offer higher brightness and the ability to display images without image burn-in.
[0006] Regarding micro LED displays, Patent Document 2 discloses a micro LED display device including a micro LED driving substrate and a micro LED panel (claim 1 of Patent Document 2).
[0007] The development of phosphor materials (fluorescent materials) applicable to these applications is also progressing. For example, Patent Document 3 discloses a phosphor having an emission maximum wavelength of 500 nm or more and 600 nm or less, a half-value width of 46 nm or less, and having the following formula: Sr 1-x Ga 2 S 4 :Eu x (where 0.10≦x≦0.20) is disclosed (claim 1 of Patent Document 3). It is also disclosed that the green-emitting phosphor can emit light with high color purity and can be used as a backlight source for a display device or a light source for illumination (paragraphs
[0008] and
[0052] of Patent Document 3).
[0008] Japanese Patent No. 5052507 Japanese Patent Application Laid-Open No. 2018-182282 Japanese Patent Application Laid-Open No. 2020-139056
[0009] Thus, while LED phosphors and their materials are used in a variety of applications, they are generally desired to have excellent emission colors, i.e., to suppress the contamination of emission colors other than those required. If unnecessary colors are contaminated, it becomes difficult to obtain the desired color tone and clear images when constructing a light-emitting device. To obtain excellent emission colors, it is important that the emission spectrum (fluorescence spectrum) is narrow and does not transmit blue light. To achieve this, a phosphor that exhibits high absorptivity (Abs.) for blue light is desired. Here, absorptivity is the proportion of irradiated light absorbed by the phosphor.
[0010] For example, as shown in Figure 1, the phosphor for a micro LED display ideally absorbs and excites all of the blue light emitted by the LED with a phosphor layer made of a green phosphor and a phosphor layer made of a red phosphor, thereby converting the color. Furthermore, the phosphor layer is small, ranging in thickness from several tens to several hundred micrometers. Therefore, even if the phosphor layer is thin, it is necessary to sufficiently absorb the emitted light (excitation light), and for this purpose, it is particularly important to increase the absorption rate of the phosphor.
[0011] However, conventional fluorescent materials for LEDs have been inadequate in meeting this demand.
[0012] The present inventors have conducted research in light of these conventional problems, and have found that, in phosphor powders (powdered fluorescent materials), there is a relationship between the fluorescence intensity ratio and the absorptance at a specific excitation wavelength in the excitation spectrum, and that increasing this fluorescence intensity ratio makes it possible to increase the absorptance of blue light.
[0013] The present invention was completed based on these findings, and aims to provide a phosphor powder that exhibits high absorptivity for blue light. Another aim of the present invention is to provide a phosphor resin composition, a phosphor, a light-emitting element, and a light-emitting device that contain the phosphor powder.
[0014] The present invention encompasses the following aspects (1) to (15). In this specification, the expression "to" includes both ends of the expression. In other words, "X to Y" is synonymous with "at least X and at most Y."
[0015] (1) In the excitation spectrum showing the fluorescence intensity at the maximum fluorescence wavelength λmax (where λmax is the fluorescence wavelength that produces the maximum fluorescence intensity for excitation light of a wavelength of 450 nm), the maximum fluorescence intensity (I 380-420 ) and the fluorescence intensity (I 450 ) and the ratio (I 450 / I 380-420 ) is 0.88 or more.
[0016] (2) In the excitation spectrum showing the fluorescence intensity at the maximum fluorescence wavelength λmax (where λmax is the fluorescence wavelength that produces the maximum fluorescence intensity for excitation light of a wavelength of 450 nm), the maximum fluorescence intensity (I 330-360 ) and the fluorescence intensity (I 450 ) and the ratio (I 450 / I 330-360 ) is 0.93 or more.
[0017] (3) In the excitation spectrum showing the fluorescence intensity at the maximum fluorescence wavelength λmax (where the maximum fluorescence wavelength λmax is the fluorescence wavelength that produces the maximum fluorescence intensity for excitation light of a wavelength of 450 nm), 450 ) and the fluorescence intensity (I 500 ) and the ratio (I 450 / I 500 ) is 1.4 or more and 2.2 or less.
[0018] (4) In the excitation spectrum showing the fluorescence intensity at the maximum fluorescence wavelength λmax (where λmax is the fluorescence wavelength that produces the maximum fluorescence intensity for excitation light of a wavelength of 450 nm), the maximum fluorescence intensity (I 380-420 ) and the fluorescence intensity (I 250 ) and the ratio (I 380-420 / I 250 ) is 2.7 or more.
[0019] (5) The phosphor powder according to any one of (1) to (4), wherein the phosphor powder contains a crystal of a host compound and a luminescent center element.
[0020] (6) The phosphor powder according to (5) above, wherein the concentration ratio of the luminescent center element is 8.0 mol % or more and 50 mol % or less.
[0021] (7) The phosphor powder according to (5) or (6) above, wherein the matrix compound contains a sulfide-based fluorescent material.
[0022] (8) The phosphor powder according to any one of (5) to (7), wherein the matrix compound contains at least one metal element selected from the group consisting of barium (Ba), strontium (Sr), and calcium (Ca), gallium (Ga), and sulfur (S).
[0023] (9) The parent compound is (Ba, Sr)Ga 2 S 4 The phosphor powder according to any one of (5) to (8) above, having a basic composition:
[0024] (10) (Ba, Sr) 1-x Ga 2 S4 :Eu x (9) A phosphor powder according to any one of (1) to (9) above, having a composition expressed by the formula (where 0.08≦x≦0.50).
[0025] (11) The phosphor powder according to any one of (1) to (10) above, which has an absorptivity of 65% or more for excitation light having a wavelength of 450 nm.
[0026] (12) A phosphor resin composition comprising the phosphor powder of any one of (1) to (11) above and a resin.
[0027] (13) A phosphor comprising the phosphor resin composition of (12) above.
[0028] (14) A light-emitting device comprising the phosphor of (13) above and an excitation source.
[0029] (15) A light-emitting device comprising the light-emitting element of (14) above.
[0030] The present invention provides a phosphor powder that exhibits high absorptivity for blue light. The present invention also provides a phosphor resin composition, a phosphor, a light-emitting element, and a light-emitting device that contain the phosphor powder.
[0031] 1 is a diagram for explaining phosphors for micro LED displays. It shows the excitation spectra of the phosphor powders of Examples 1 to 3. It shows the excitation spectra of the phosphor powders of Examples 4 to 6. It shows the excitation spectra of the phosphor powders of Examples 7 and 8. It shows the excitation spectra of the phosphor powders of Comparative Examples 1 to 3.
[0032] A specific embodiment of the present invention (hereinafter referred to as the "present embodiment") will be described. Note that the present invention is not limited to the following embodiment, and various modifications are possible within the scope of the present invention.
[0033] <<1. Phosphor Powder>> The phosphor powder of the present embodiment includes one or more of the following first to fourth aspects.
[0034] <First Aspect> The phosphor powder according to the first aspect has an excitation spectrum showing the fluorescence intensity at the maximum fluorescence wavelength λmax, in which the maximum fluorescence intensity (I 380-420) and the fluorescence intensity (I 450 ) and the ratio (I 450 / I 380-420 ) is 0.88 or more. Here, the maximum fluorescence wavelength λmax is a fluorescence wavelength that produces a maximum fluorescence intensity with respect to excitation light of a wavelength of 450 nm. In other words, in the excitation spectrum showing the fluorescence intensity of the maximum fluorescence wavelength λmax (where the maximum fluorescence wavelength λmax is a fluorescence wavelength that produces a maximum fluorescence intensity in an emission spectrum (fluorescence spectrum) measured with excitation light of a wavelength of 450 nm), the maximum fluorescence intensity (I 380-420 ) and the fluorescence intensity (I 450 ) and the ratio (I 450 / I 380-420 ) is 0.88 or more.
[0035] Fluorescence intensity ratio (I 450 / I 380-420 ), the absorption rate of blue light increases, and as a result, the transmission of blue light can be suppressed. This is because the luminescent center element (Eu) in the host crystal 2+ There are multiple energy levels in the nucleus, but the nucleus is located at an energy of 450 nm. 7 F 3 The proportion of the state 7 F 6 or 7 F 5 It is presumed that this is because the absorption rate of blue light increases when the fluorescence intensity is increased to a level higher than that of the excitation light with a wavelength of 450 nm. 450 / I 380-420 ) was used as an index because the emission wavelength of blue LEDs, which are most frequently used as excitation sources for LED phosphors, is 450 nm.
[0036] Furthermore, the fluorescence intensity ratio (I 450 / I 380-420 By increasing the fluorescence intensity ratio (I), it is possible to increase the degree of freedom in designing the light-emitting device. That is, in addition to an LED with an emission wavelength of 450 nm, an LED with an emission wavelength of around 460 nm may also be used as an excitation source for the phosphor. 450 / I 380-420By increasing the fluorescence intensity ratio (I 450 / I 380-420 The fluorescence intensity ratio (I) is preferably 0.90 or more, and more preferably 0.91 or more. 450 / I 380-420 The upper limit of the fluorescence intensity ratio (I 450 / I 380-420 ) is preferably 0.88 or more and 1.00 or less, and more preferably 0.91 or more and 1.00 or less.
[0037] Fluorescence intensity ratio (I 450 / I 380-420 ) can be determined by the following procedure. First, the phosphor powder is analyzed using a spectrofluorometer to determine the fluorescence spectrum (emission spectrum; PL spectrum). The fluorescence spectrum is a spectrum of fluorescence intensity obtained by fixing the excitation light wavelength at a specific value and scanning the fluorescence wavelength. By examining the fluorescence spectrum, it is possible to determine which wavelength of the light emitted by the phosphor is the most intense. Then, in the obtained fluorescence spectrum, the wavelength that produces the maximum (maximum) fluorescence luminosity (maximum fluorescence wavelength λmax) is determined. For phosphor powders that emit green light (green phosphor powders), λmax is typically in the range of 490 nm to 550 nm (e.g., 535 nm).
[0038] Next, the phosphor powder is analyzed using a spectrofluorometer to obtain an excitation spectrum (PLE spectrum). The excitation spectrum is a spectrum of fluorescence intensity obtained by fixing the fluorescence wavelength (the emission wavelength emitted from the phosphor) to a specific value and scanning the wavelength of excitation light incident on the phosphor. By examining the excitation spectrum, it is possible to determine which wavelength of excitation will produce the strongest fluorescence, i.e., the optimal excitation wavelength. In this embodiment, the excitation spectrum is obtained by fixing the fluorescence wavelength to the maximum fluorescence wavelength λmax.
[0039] Thereafter, in the obtained excitation spectrum, the maximum fluorescence intensity (I 380-420) and the fluorescence intensity (I 450 ) is calculated. Here, the maximum fluorescence intensity (I 380-420 ) is the maximum fluorescence intensity within the excitation light wavelength range of 380 nm to 420 nm. 450 ) is the fluorescence intensity when the excitation light wavelength is 450 nm. 380-420 and I 450 From this, the fluorescence intensity ratio (I 450 / I 380-420 ) is calculated.
[0040] <Second Aspect> The phosphor powder according to the second aspect has an excitation spectrum showing the fluorescence intensity at the maximum fluorescence wavelength λmax, in which the maximum fluorescence intensity (I 330-360 ) and the fluorescence intensity (I 450 ) and the ratio (I 450 / I 330-360 ) is 0.93 or more. Here, the maximum fluorescence wavelength λmax is as explained in the first embodiment. 330-360 ) is the maximum fluorescence intensity within the excitation light wavelength range of 330 nm or more and 360 nm or less. In other words, in the excitation spectrum showing the fluorescence intensity of the maximum fluorescence wavelength λmax (where the maximum fluorescence wavelength λmax is the fluorescence wavelength that brings about the maximum fluorescence intensity in the emission spectrum (fluorescence spectrum) measured with excitation light of a wavelength of 450 nm), the maximum fluorescence intensity (I 330-360 ) and the fluorescence intensity (I 450 ) and the ratio (I 450 / I 330-360 ) is 0.93 or more.
[0041] Fluorescence intensity ratio (I 450 / I 330-360 ) in the host crystal, the absorption rate of blue light is further increased. 2+ There are multiple 5d orbitals in fluorescein, but the maximum fluorescence intensity (I 330-360 ) affecting 5d xy , 5d x^2-y^2The fluorescence intensity (I 450 ) affecting 5d Z^2 It is presumed that this is because the absorption rate of blue light increases by increasing the proportion of 450 / I 330-360 The fluorescence intensity ratio (I) is more preferably 0.95 or more, and even more preferably 0.96 or more. 450 / I 330-360 The upper limit of the fluorescence intensity ratio (I 450 / I 330-360 ) is preferably 0.93 or more and 2.00 or less, more preferably 0.95 or more and 2.00 or less, and even more preferably 0.96 or more and 2.00 or less.
[0042] <Third Aspect> The phosphor powder according to the third aspect has an excitation spectrum showing a fluorescence intensity at a maximum fluorescence wavelength λmax, in which the fluorescence intensity (I 450 ) and the fluorescence intensity (I 500 ) and the ratio (I 450 / I 500 ) is 1.4 or more and 2.2 or less. Here, the maximum fluorescence wavelength λmax is as described in the first embodiment. That is, in the excitation spectrum showing the fluorescence intensity of the maximum fluorescence wavelength λmax (where the maximum fluorescence wavelength λmax is the fluorescence wavelength that gives the maximum fluorescence intensity in the emission spectrum (fluorescence spectrum) measured with excitation light of a wavelength of 450 nm), the fluorescence intensity (I 450 ) and the fluorescence intensity (I 500 ) and the ratio (I 450 / I 500 ) is 1.4 or more and 2.2 or less.
[0043] Fluorescence intensity ratio (I 450 / I 500) within the aforementioned range, the absorptance of blue light is further increased. The reason for this is that the wavelength of 500 nm overlaps with the emission wavelength of the green phosphor. In other words, if the absorptance at this wavelength (500 nm) becomes high, the phosphor will reabsorb the converted light, which is thought to reduce the luminescence performance. Therefore, it is presumed that the excitation intensity at 500 nm needs to be appropriately lower than that at 450 nm. From the viewpoint of increasing the absorptance, the fluorescence intensity ratio (I 450 / I 500 ) is more preferably 1.6 or more and 2.0 or less.
[0044] <Fourth Aspect> The phosphor powder according to the fourth aspect has an excitation spectrum showing a fluorescence intensity at a maximum fluorescence wavelength λmax, in which the maximum fluorescence intensity (I 380-420 ) and the fluorescence intensity (I 250 ) and the ratio (I 380-420 / I 250 ) is 2.7 or more. Here, the maximum fluorescence wavelength λmax is as explained in the first aspect. That is, in the excitation spectrum showing the fluorescence intensity of the maximum fluorescence wavelength λmax (where the maximum fluorescence wavelength λmax is the fluorescence wavelength that gives the maximum fluorescence intensity in the emission spectrum (fluorescence spectrum) measured with excitation light of a wavelength of 450 nm), the maximum fluorescence intensity (I 380-420 ) and the fluorescence intensity (I 250 ) and the ratio (I 380-420 / I 250 ) is 2.7 or more.
[0045] Fluorescence intensity ratio (I 380-420 / I 250 By limiting the wavelength of Eu within the above range, the absorption rate of blue light is further increased. This is because the 250 nm region corresponds to the excitation band of the host compound, and the luminescent center element (Eu 2+ It is speculated that the higher the concentration of the excited parent compound, the lower the probability of the parent compound being excited. 380-420 / I 250The fluorescence intensity ratio (I) is more preferably 2.8 or more, and even more preferably 2.9 or more. 380-420 / I 250 The upper limit of the fluorescence intensity ratio (I) is not limited. However, it is typically 5.0 or less. 380-420 / I 250 ) is preferably 2.7 or more and 5.0 or less, more preferably 2.8 or more and 5.0 or less, and even more preferably 2.9 or more and 5.0 or less.
[0046] The phosphor powder of this embodiment satisfies at least one of the requirements defined in the first to fourth aspects described above. That is, it may satisfy only one of the requirements, or two or more of the requirements, or all of the requirements. When two or more of the requirements are satisfied, any two or more of the first to fourth aspects may be combined to satisfy the requirements.
[0047] The phosphor powder of this embodiment is not limited in its material composition as long as it exhibits fluorescent properties. The phosphor powder is made of a fluorescent material and generally contains a crystal of a host compound and a luminescent center element (activator). Known fluorescent materials include oxide-based, sulfide-based, oxysulfide-based, nitride-based, and oxynitride-based materials, and any of these may be used.
[0048] For example, oxide-based fluorescent materials (Y, Gd, Lu) 3 (Al, Ga) 5 O 12 : Ce 3+ , (Ba, Sr, Ca) 2 SiO 4 :Eu 2+ , (Ba, Sr, Ca) 3 MgSi 2 O 8 :Eu 2+ , CaAl 12 O 19 : Mn 4+ , Ca 3 Sc 2 Si 3 O 12 : Ce 3+ , CaSc 2 O 4 : Ce 3+ , (Ba, Sr) 3 SiO 5 :Eu2+ , Li 2 SrSiO 4 :Eu 2+ , Ba 9 Sc 2 Si 6 O 24 :Eu 2+ , Ca 3 Si 2 O 7 :Eu 2+ , LiSrPO 4 :Eu 2+ , CaLa 4 Si 3 O 13 :Eu 3+ , Ba 2 Gd 3 Li 3 Mo 8 O 32 :Eu 3+ and BaMgAl 10 O 17 :Eu 2+ , Mn 2+ Examples include:
[0049] Sulfide-based fluorescent materials: (Ba, Sr, Ca)Ga 2 S 4 :Eu 2+ , (Ba,Sr,Ca)Ga 2 S 4 : Ce 3+ , (Sr,Ca)S:Eu 2+ , (Sr,Cd)S:Eu 2+ and ZnS:Cu.
[0050] As oxysulfide fluorescent materials (La, Y) 2 O 2 S: EU 3+ and La(Ca,Sr)Ga 3 S 6 O:Eu 2+ Examples include:
[0051] Nitride-based fluorescent materials (Ba, Sr, Ca) 2 Si 5 N 8 :Eu 2+ , (Ba,Ca,Sr)AlSiN 3 :Eu 2+ , La3 Si 6 N 11 : Ce 3+ , (Ba,Sr,Ca)LiAl 3 N 4 :Eu 2+ , Sr(Mg 3 SiN 4 ): Eu 2+ and (Ba, Sr) 2 Si 5 N 8 :Eu 2+ Examples include:
[0052] As oxynitride fluorescent materials, Eu-containing α-type sialon, Eu-containing β-type sialon, Ba 9 Sc 3 Si 6 O 21 N 3 :Eu 2+ , Ba 3 Si 6 O 12 N 2 :Eu 2+ , BaSi 2 O 2 N 2 :Eu 2+ and (Ba, Sr, Ca)AlSi(ON) 3 :Eu 2+ Examples include:
[0053] Other fluorescent materials include Sr 10 (P.O. 4 ) 6 C 12 :Eu 2+ and K. 2 (Si,Ge,Ti)F 6 : Mn 4+ Examples include:
[0054] According to a preferred embodiment, the phosphor powder contains a host compound containing at least one metal element selected from the group consisting of barium (Ba), strontium (Sr), and calcium (Ca), gallium (Ga), and sulfur (S), as well as a luminescent center element, as in the composition listed above for the sulfide-based fluorescent material. More preferably, the host compound is (Ba,Sr)Ga. 2 S 4Preferably, the luminescent center element contains at least one element selected from the group consisting of europium (Eu), cerium (Ce), manganese (Mn), and samarium (Sm). From the viewpoint of increasing the internal quantum efficiency (IQE) upon excitation by blue light emitted from the LED, the luminescent center element preferably contains Eu, and divalent ions of Eu (Eu 2+ ), and more preferably, Eu 2+ It is more preferred that the composition contains only:
[0055] Assuming that the phosphor powder satisfies the requirements for the fluorescence intensity ratio defined in the first to fourth aspects described above, the content of the luminescent center element in the phosphor powder is not limited. However, from the viewpoint of more reliably and easily satisfying the above requirements, it is preferable that the luminescent center element is solid-dissolved at a high concentration in the phosphor powder. By solid-dissolving the luminescent center element at a high concentration, a high fluorescence intensity ratio (I 450 / I 380-420 It is possible to realize the desired absorption rate and the like. Regardless of the composition of the phosphor powder, the concentration ratio of the luminescent center element is preferably 8.0 mol % or more and 50 mol % or less. Here, the concentration ratio of the luminescent center element is the ratio (XA / (XM+XA)) of the molar amount of the luminescent center element (XA) to the sum of the molar amount of the host compound (XM) and the molar amount of the luminescent center element (XA) contained in the phosphor powder. The higher the concentration ratio of the luminescent center element, the higher the ratio (I 450 / I 380-420 ) becomes higher, resulting in higher absorptance of blue light. From the viewpoint of increasing absorptance, the concentration ratio is preferably 12 mol% or more, more preferably 13 mol% or more. On the other hand, if the concentration ratio becomes too high, the luminescent center element may not be completely dissolved in the host compound, and a heterophase may be formed. The formation of a heterophase may cause problems such as a decrease in luminescence intensity. From the viewpoint of suppressing the formation of a heterophase, the concentration ratio is preferably 45 mol% or less, more preferably 40 mol% or less. From the viewpoint of suppressing the formation of a heterophase while increasing absorptance, the concentration ratio is preferably 12 mol% or more and 45 mol% or less, more preferably 13 mol% or more and 40 mol% or less.
[0056] According to a preferred embodiment, the phosphor powder is (Ba, Sr) 1-x Ga 2 S4 :Eu x (where 0.08≦x≦0.50). This phosphor powder contains a thiogallate compound as a host compound and europium (Eu) as a luminescent center element, and emits green light when excited by excitation light with a wavelength in the near-ultraviolet to blue region (approximately 300 nm to 510 nm). Furthermore, since it contains a relatively high concentration of the luminescent center element (Eu), it is possible to exhibit high absorptivity for blue light. From the viewpoint of increasing absorptivity, the Eu amount x is preferably 0.12 or more, and more preferably 0.13 or more. From the viewpoint of suppressing heterophase formation, x is preferably 0.45 or less, and more preferably 0.40 or less. From the viewpoint of suppressing heterophase formation while increasing absorptivity, the Eu amount x is preferably 0.12 or more and 0.45 or less, and even more preferably 0.13 or more and 0.40 or less.
[0057] According to a further preferred embodiment, the phosphor powder is (Ba y Sr 1-y ) 1-x Ga z S 4 :Eu x (where 0.08≦x≦0.50, 0.00≦y≦1.00, 1.5≦z≦2.5). This phosphor powder contains a relatively high concentration of the luminescent center element (Eu), and is therefore able to exhibit high absorptivity for blue light. From the viewpoint of increasing absorptivity, the Eu amount x is preferably 0.12 or more, and more preferably 0.13 or more. From the viewpoint of suppressing the formation of heterophases, x is preferably 0.45 or less, and more preferably 0.40 or less. From the viewpoint of increasing absorptivity, the Ba amount y is preferably 0.50 or less, and more preferably 0.30 or less. From the viewpoint of suppressing the formation of heterophases, the Ga amount z is preferably 1.7 or more and 2.3 or less.
[0058] The phosphor powder may or may not have a coating layer. By providing a coating layer, durability such as moisture resistance can be improved. From the viewpoint of improving durability while maintaining the good luminescence properties of the phosphor, the coating layer is preferably made of silicon dioxide (SiO 2 ), zinc oxide (ZnO), aluminum oxide (Al 2 O 3 ), titanium oxide (TiO 2), and / or oxides containing boron (B), barium sulfate (BaSO 4 It is preferable that the inorganic compound is composed of one or more inorganic compounds such as metal sulfates.
[0059] The phosphor powder may contain components other than the fluorescent material, such as a flux component such as a sintering aid that is added during the synthesis of the phosphor powder.
[0060] The phosphor powder of this embodiment has a high fluorescence intensity ratio in at least one of the first to fourth aspects described above, and therefore a high absorptance of blue light. As a result, the emission spectrum (fluorescence spectrum) is narrow and the emitted light color is excellent. From the viewpoint of obtaining a better emitted light color, the higher the absorptance for excitation light with a wavelength of 450 nm, the more preferable. Specifically, the absorptance is preferably 65% or more, more preferably 69% or more, and even more preferably 75% or more. There is no upper limit to the absorptance; it is sufficient as long as it is 100% or less. However, for some applications such as lighting and mini LED displays, it may not be necessary to increase the absorptance to 100%. In such cases, the absorptance may be 95% or less. The absorptance is preferably 65% to 100%, more preferably 69% to 100%, and even more preferably 75% to 95%.
[0061] <<2. Manufacturing Method of Phosphor Powder>> The manufacturing method of the phosphor powder of this embodiment is not limited, provided that the above-mentioned requirements are satisfied. However, it is preferable to manufacture the phosphor powder by a method that dissolves the luminescent center element in the host compound at a high concentration, increases the crystallinity of the host compound, and further reduces distortion. A specific preferred manufacturing method includes a step of mixing raw materials to prepare a raw material mixture (raw material mixing step), and a step of firing the obtained raw material mixture (firing step). Furthermore, from the viewpoint of easily promoting the solid solution of the luminescent center element and improving the crystallinity of the host compound, it is preferable to reduce (slow) the temperature rise rate when firing the raw material mixture and to raise the firing temperature to a certain level. When the phosphor powder is (Ba, Sr), 1-x Ga 2 S 4 :Eu xA preferred manufacturing method will be described in detail below, taking as an example a case where the composition is expressed as (where 0.08≦x≦0.50).
[0062] <Raw Material Mixing Step> In the raw material mixing step, raw materials are mixed to prepare a raw material mixture. 1-x Ga 2 S 4 :Eu x In the case where the phosphor powder has a composition represented by the formula (1), a barium (Ba) raw material, a strontium (Sr) raw material, a gallium (Ga) raw material, a europium (Eu) raw material, and optionally a sulfur (S) raw material are weighed and mixed. The blending ratio of the raw materials is determined so that the composition of the phosphor powder finally obtained is (Ba, Sr) 1-x Ga 2 S 4 :Eu x (where x is 0.08≦x≦0.50). The raw material may contain only one of the elements (constituent elements) that make up the phosphor powder, or may contain a combination of multiple constituent elements. When a solid component is used as the sulfur raw material, the sulfur raw material may be mixed. When a gas component is used as the sulfur raw material, the sulfur raw material does not need to be mixed.
[0063] Examples of the barium and strontium raw materials include oxides, sulfides, double oxides, and / or carbonates of the respective elements. Examples of the gallium raw material include oxides (Ga 2 O 3 Examples of sulfur raw materials include strontium sulfide (SrS), barium sulfide (BaS), sulfur (S), silicon sulfide (SiS 2 ), cerium sulfide (Ce 2 S 3 ), and / or hydrogen sulfide (H 2 S) gas. Europium raw material includes europium fluoride (EuF 3 ), europium oxide (Eu 2 O 3 ), and / or europium chloride (EuCl 3 ) are listed.
[0064] In order to adjust the emission wavelength of the phosphor powder and improve the external quantum efficiency (EQE), rare earth elements such as praseodymium (Pr) and samarium (Sm) may be added to the raw materials. Furthermore, in order to improve the excitation efficiency, at least one element selected from rare earth elements such as scandium (Sc), lanthanum (La), gadolinium (Gd), and lutetium (Lu) may be added to the raw materials as a sensitizer. However, it is preferable that the amount of each of these elements be 5 mol % or less relative to strontium (Sr). By keeping the content of these elements at 5 mol % or less, it is possible to prevent a large amount of heterophase from precipitating, and thus a significant decrease in brightness. Furthermore, alkali metal elements, silver ions (Ag + Monovalent cations such as Cr (Cu), Cr (Cu), and halogen ions such as chlorine (Cl), fluorine (F), and iodine (I) may be added to the raw material as charge compensation agents. In terms of charge compensation effect and brightness, the amount of the added agent is preferably approximately equal to the content of the aluminum group element or rare earth element.
[0065] The raw material mixing method is not limited. Either a dry method or a wet method may be used. In the case of dry mixing, for example, the raw material mixture may be prepared by mixing the raw materials in a mixer such as a paint shaker or a ball mill using zirconia balls as media, and drying as necessary. In the case of wet mixing, for example, a solvent such as water is added to the raw materials to form a suspension, and the suspension is mixed in a mixer such as a paint shaker or a ball mill using zirconia balls as media, followed by separating the media using a sieve or the like, and then removing the solvent from the suspension by a drying method such as reduced pressure drying or vacuum drying.
[0066] The resulting raw material mixture is then fired to produce a fired product. If necessary, the raw material mixture may or may not be pulverized, classified, and / or dried before firing.
[0067] Luminescent center element (Eu 2+From the viewpoint of promoting solid dissolution of the luminescent center element (e.g., etc.) and improving the crystallinity of the host compound, it is preferable to reduce the heating rate when firing the raw material mixture and increase the firing temperature to a certain extent. If the heating rate is too high or the firing temperature is too low, the solid dissolution of the luminescent center element may not proceed, and a different phase may remain in the final phosphor powder. Furthermore, the crystallinity of the host compound may decrease, resulting in residual distortion. On the other hand, if the heating rate is too low or the firing temperature is too high, the process may take longer and productivity may decrease. Furthermore, the constituent elements in the raw material mixture may volatilize, resulting in compositional deviation of the phosphor powder. The heating rate is preferably 0.05°C / min or more and 5°C / min or less, more preferably 0.1°C / min or more and 0.4°C / min or less. The firing temperature is preferably 900°C or more and 1200°C or less, more preferably 1050°C or more and 1150°C or less. The firing holding time is preferably 24 hours or more and 168 hours or less.
[0068] The firing atmosphere may be an inert gas or a reducing gas, etc. Examples include an argon atmosphere, a nitrogen atmosphere, a sulfur atmosphere, an argon atmosphere containing hydrogen gas, a nitrogen atmosphere containing hydrogen gas, a hydrogen sulfide atmosphere, etc. Among these, firing in a hydrogen sulfide atmosphere is preferred.
[0069] When the raw material mixture contains a sulfur (S) raw material, it can be calcined under an atmosphere of hydrogen sulfide, carbon disulfide, or an inert gas. When hydrogen sulfide or carbon disulfide is used, these become sulfur compounds during calcination, which have the effect of suppressing decomposition of the product. On the other hand, when the raw material does not contain a sulfur raw material, it is preferable to calcinate under a sulfur-containing atmosphere such as hydrogen sulfide or carbon disulfide.
[0070] The fired product is then crushed into powder. Crushing can be performed either dry or wet. In the wet method, ethanol, water, or the like can be used as a dispersion medium. Crushing can be performed using a known crusher such as a ball mill, stamp mill, jet mill, crusher, and / or paint shaker. If necessary, the crushed product obtained by crushing can be classified. When performing classification, the particle size of the product is preferably 0.01 μm to 150 μm, more preferably 1 μm to 50 μm, from the viewpoint of improving the handleability and luminescence of the resulting phosphor. Note that the particle size here refers to the particle size (D50) at 50% cumulative volume as measured by a laser diffraction / scattering particle size distribution measurement method. In this manner, the phosphor powder of this embodiment can be obtained.
[0071] <<3. Phosphor Resin Composition>> The phosphor resin composition of this embodiment contains the above-described phosphor powder and a resin. The phosphor resin composition is a phosphor paste that is a precursor of a phosphor. The phosphor is produced by applying or molding the phosphor resin composition.
[0072] The resin may be, for example, one or more selected from thermoplastic resins, thermosetting resins, ionizing radiation curable resins, and two-component curable resins. Examples of thermoplastic resins include polyolefin resins such as polyethylene and polypropylene; polyester resins such as polyethylene terephthalate and polybutylene terephthalate; polycarbonate resins; polyacrylic acid resins such as polyacrylic acid or its esters, polymethacrylic acid or its esters; polyvinyl resins such as polystyrene and polyvinyl chloride; cellulose resins such as triacetyl cellulose; and urethane resins such as polyurethane. Examples of thermosetting resins include silicone resins, phenolic resins, epoxy resins, melamine resins, urea resins, unsaturated polyester resins, alkyd resins, polyurethane resins, and polyimide resins. Examples of ionizing radiation curable resins include acrylic resins, urethane resins, vinyl ester resins, and polyester alkyd resins. These resins may be used not only as polymers but also as oligomers or monomers. Examples of two-component curable resins include epoxy resins.
[0073] The amount of phosphor powder contained in the phosphor resin composition is preferably 5 parts by mass or more, more preferably 20 parts by mass or more, per 100 parts by mass of resin, from the viewpoint of easily ensuring absorptivity while obtaining sufficient external quantum efficiency, while being 100 parts by mass or less, more preferably 70 parts by mass or less, per 100 parts by mass of resin, from the viewpoint of ensuring favorable moldability (fillability).
[0074] The phosphor resin composition may contain an organic solvent, an additive, and the like. The viscosity of the phosphor resin composition (phosphor paste) can be adjusted by adding an organic solvent. Any known organic solvent that dissolves resins may be used. As the additive, an inorganic filler such as glass particles or metal oxide particles, or a flow adjuster made of an organic component may be used.
[0075] The phosphor resin composition is produced by mixing and kneading a phosphor powder, a resin, and, if necessary, an organic solvent and additives. The mixing and kneading may be performed using known means, such as a triple roll mill, a kneader, a single- or double-screw kneader, a revolution-type stirring and degassing device, and / or a planetary mill. The resulting phosphor resin composition is used as a phosphor paste for producing a phosphor.
[0076] <<4. Phosphor>> The phosphor of this embodiment is a molded body of the phosphor resin composition described above. The molded body is a concept that includes coatings and fillers obtained from the composition. That is, the phosphor resin composition (phosphor paste) is applied, filled, or molded, and then dried and / or cured as necessary to produce a phosphor. The phosphor has phosphor powder (particles) dispersed in a resin matrix.
[0077] <<5. Light-Emitting Element>> The light-emitting element of this embodiment includes the above-described phosphor and an excitation source. The excitation source emits light toward the phosphor to excite it. An LED with a central wavelength of 250 nm to 510 nm, particularly a blue LED with a central wavelength of 450 nm to 460 nm, is suitable as the excitation source. The arrangement of the phosphor and excitation source is not limited as long as light from the excitation source is incident on the phosphor. However, it is preferable to arrange the phosphor directly above the excitation source. This allows the phosphor to more efficiently absorb the light emitted from the excitation source and perform color conversion. For example, when the light-emitting element is applied to a micro LED display, it is preferable to arrange the LED as the excitation source below and the phosphor above it within each package rib of the display. While quantum dots can also be used as components of a light-emitting element instead of phosphors, quantum dots often contain environmentally restricted substances. Furthermore, due to their poor durability, phosphors are more advantageous.
[0078] <<6. Light-Emitting Device>> The light-emitting device of this embodiment includes the light-emitting element described above. The light-emitting device is not particularly limited as long as it includes a phosphor light-emitting element. Examples include display devices such as displays and lighting. Examples of display devices include, but are not limited to, micro LED displays and mini LED displays.
[0079] A micro LED display is particularly suitable as the light-emitting device of this embodiment. Micro LED displays, which have a small phosphor layer (phosphor) thickness of tens to hundreds of μm, are required to sufficiently absorb emitted light (excitation light) to obtain an excellent emission color. The light-emitting element of this embodiment has a high absorption rate of the phosphor provided therein, resulting in an excellent emission color. Therefore, the above-mentioned requirements are met.
[0080] The present invention will be described in more detail using the following examples, but the present invention is not limited to the following examples.
[0081] (1) Preparation of Phosphor Powder [Examples 1 to 8 and Comparative Examples 1 to 3] Barium sulfide (BaS), strontium sulfide (SrS), europium sulfide (EuS), and gallium sulfide (Ga 2 S3 ) were prepared and weighed out so as to obtain the molar ratios of Eu (Eu / (Ba+Sr+Eu); luminescence center element concentration ratio), Ba (Ba / (Ba+Sr)), and Ga (Ga / (Eu+Ba+Sr)) shown in Table 1 below. Next, the weighed materials were mixed for 100 minutes using a paint shaker with a zirconia ball having a diameter of 3 mm to obtain a raw material mixture. Thereafter, the obtained raw material mixture was mixed with hydrogen sulfide (H 2 The firing was carried out under the conditions (heating rate, firing temperature, and firing time) shown in Table 1 below.
[0082] 50 g of the resulting fired product and 50 g of ethanol were placed in a 500 mL alumina pot to obtain a mixed solution with a solid content of 50% by mass. The mixture was then subjected to wet crushing using a ball mill to obtain a crushed phosphor powder. During the crushing process, 300 g of zirconia balls with a diameter of 7 mm and 400 g of zirconia balls with a diameter of 3 mm were used. The ball rotation speed was 300 rpm, and the treatment time using the ball mill was 4 hours.
[0083] The resulting phosphor powder (crushed material) was dissolved in acid and subjected to composition analysis by ICP-OES, which confirmed that the phosphor powder composition was substantially the same as the charged composition.
[0084] (2) Evaluation The phosphor powders obtained in Examples 1 to 8 and Comparative Examples 1 to 3 were evaluated for various properties as follows.
[0085] <Fluorescence Spectra and Excitation Spectra> Fluorescence spectra and excitation spectra were determined for the phosphor powders (samples) obtained in the Examples and Comparative Examples as follows. Specifically, measurements and analyses were performed using a spectrofluorometer FP-8500 and an integrating sphere unit ISF-834 (manufactured by JASCO Corporation) according to a solid-state quantum efficiency calculation program. The spectrofluorometer was calibrated using a secondary standard light source and rhodamine B. The fluorescence spectra and excitation spectra were determined under the following conditions: excitation and fluorescence bandwidths of 5 nm each, a scanning speed of 500 nm / min, a data acquisition interval of 0.2 nm, and a response time of 1 second. When measuring the fluorescence spectra, the wavelength of the excitation light was fixed at 450 nm, and the fluorescence wavelength was scanned to determine the wavelength that yielded the maximum (maximum) fluorescence intensity on the spectrum (maximum fluorescence wavelength λmax). Furthermore, when measuring the excitation spectrum, the excitation light wavelength was scanned to determine the spectrum showing the fluorescence intensity at the maximum fluorescence wavelength λmax.
[0086] Next, in the obtained excitation spectrum, the fluorescence intensity (I 250 ), the fluorescence intensity (I 450 ), the fluorescence intensity (I 500 ), the maximum fluorescence intensity (I 330-360 ), and the maximum fluorescence intensity (I 380-420 ) and the fluorescence intensity ratio (I 450 / I 380-420 , I 450 / I 330-360 , I 450 / I 500 and I 380-420 / I 250 ) was calculated.
[0087] <Absorptance> Using a phosphor powder (sample) as a sample for absorptance measurement, the absorptance (Abs.) was measured as follows. Specifically, measurements and analysis were performed using a FP-8500 spectrofluorometer and an ISF-834 integrating sphere unit (manufactured by JASCO Corporation) in accordance with a solid-state quantum efficiency calculation program. The spectrofluorometer was calibrated using a secondary standard light source and rhodamine B. The formula for calculating the absorptance of the phosphor powder (sample) is shown below, assuming an excitation light of 450 nm under the following conditions: excitation and fluorescence bandwidths of 5 nm each, a scan speed of 500 nm / min, a data acquisition interval of 0.2 nm, and a response of 1 second. This formula conforms to the description in the instruction manual for the FWSQ-6-17(32) solid-state quantum efficiency calculation program (manufactured by JASCO Corporation).
[0088] Let P1(λ) be the standard white board spectrum and P2(λ) be the sample spectrum. The area L1 (see formula (i) below) of spectrum P1(λ) surrounded by the excitation wavelength range of 433 nm to 472 nm is taken as the excitation intensity. The area L2 (see formula (ii) below) of spectrum P2(λ) surrounded by the excitation wavelength range of 433 nm to 472 nm is taken as the sample scattering intensity.
[0089]
[0090] The absorptance (Abs.) is the ratio of the excitation light attenuated by the sample to the incident light, and is calculated according to the following formula (iii).
[0091]
[0092] (3) Evaluation Results For Examples 1 to 8 and Comparative Examples 1 to 3, the fluorescence intensity ratio (I 450 / I 380-420 , I 450 / I 330-360 , I 450 / I 500 and I 380-420 / I 250 ), and absorptance (Abs.) are shown together with the manufacturing conditions of the phosphor powder (Eu amount, heating rate, firing temperature, etc.). The excitation spectra of Examples 1 to 8 and Comparative Examples 1 to 3 are shown in Figures 2 to 5.
[0093] Examples 1 to 8 are samples with a high Eu content of 0.08 to 0.30, and were prepared by firing at a relatively high temperature (1100°C). All samples except for Example 7 were prepared at a relatively low heating rate (0.3°C / min). In these samples, the fluorescence intensity ratio (I 450 / I 380-420 ) is 0.88 or more, and the fluorescence intensity ratio (I 450 / I 330-360 ) is 0.93 or more, and the fluorescence intensity ratio (I 450 / I 500 ) is 1.4 or more and 2.2 or less, and the fluorescence intensity ratio (I 380-420 / I 250 ) was 2.7 or more, and the absorption rate was accordingly high at 69% or more.
[0094] In contrast, Comparative Examples 1 and 2 are samples prepared with a low Eu content of 0.01 to 0.07 and a high temperature rise rate (5°C / min). 450 / I 380-420 is low at 0.86 or less, and I 450 / I 330-360 is 0.92 or less, and I 450 / I 500 is less than 1.4 or more than 2.2, and I 380-420 / I 250 was 2.6 or less, and the absorption rate was accordingly low at 61% or less.
[0095] Comparative Example 3 is a sample prepared by firing at a relatively low temperature (850°C) although the Eu content is as high as 0.13. 450 / I 380-420 is low at 0.87, and I 450 / I 330-360 is 0.90, and I 450 / I 500 is low at 1.37, and I 380-420 / I 250 The absorption rate was correspondingly low at 64%.
[0096] From the above results, it can be seen that this embodiment provides a phosphor powder that exhibits high absorptivity for blue light.
[0097]
Claims
1. In an excitation spectrum showing the fluorescence intensity of the maximum fluorescence wavelength λmax (where λmax is the fluorescence wavelength that produces the maximum fluorescence intensity for excitation light of a wavelength of 450 nm), the maximum fluorescence intensity (I 380-420 ) and the fluorescence intensity (I 450 ) and the ratio (I 450 / I 380-420 ) is 0.88 or more.
2. In the excitation spectrum showing the fluorescence intensity of the maximum fluorescence wavelength λmax (where λmax is the fluorescence wavelength that produces the maximum fluorescence intensity for excitation light of a wavelength of 450 nm), the maximum fluorescence intensity (I 330-360 ) and the fluorescence intensity (I 450 ) and the ratio (I 450 / I 330-360 ) is 0.93 or more.
3. In the excitation spectrum showing the fluorescence intensity at the maximum fluorescence wavelength λmax (where λmax is the fluorescence wavelength that produces the maximum fluorescence intensity for excitation light of a wavelength of 450 nm), 450 ) and the fluorescence intensity (I 500 ) and the ratio (I 450 / I 500 ) is 1.4 or more and 2.2 or less.
4. In the excitation spectrum showing the fluorescence intensity of the maximum fluorescence wavelength λmax (wherein the maximum fluorescence wavelength λmax is the fluorescence wavelength that produces the maximum fluorescence intensity for the excitation light of a wavelength of 450 nm), the maximum fluorescence intensity (I 380-420 ) and the fluorescence intensity (I 250 ) and the ratio (I 380-420 / I 250 ) is 2.7 or more.
5. The phosphor powder according to any one of claims 1 to 4, which contains a crystal of a host compound and a luminescent center element.
6. The phosphor powder according to claim 5, wherein the concentration ratio of the luminescent center element is 8.0 mol % or more and 50 mol % or less.
7. The phosphor powder according to claim 5, wherein the host compound comprises a sulfide-based phosphor material.
8. The phosphor powder according to claim 5, wherein the matrix compound contains at least one metal element selected from the group consisting of barium (Ba), strontium (Sr) and calcium (Ca), gallium (Ga) and sulfur (S).
9. The parent compound is (Ba,Sr)Ga 2 S 4 6. The phosphor powder of claim 5 having a basic composition:
10. (Ba, Sr) 1-x G 2 S 4 :Eu x 5. The phosphor powder according to claim 1, having a composition expressed by the formula: (wherein 0.08≦x≦0.50).
11. The phosphor powder according to any one of claims 1 to 4, which has an absorptivity of 65% or more for excitation light with a wavelength of 450 nm.
12. A phosphor resin composition comprising the phosphor powder according to any one of claims 1 to 4 and a resin.
13. A phosphor comprising the phosphor resin composition according to claim 12.
14. A light-emitting device comprising the phosphor according to claim 13 and an excitation source.
15. A light emitting device comprising the light emitting element according to claim 14.
Citation Information
Patent Citations
Liminous oxide having stuffed tridymite type or kaliphilite type structure and oxide luminophor
JP2000026854A
Light emitting device, lighting device and image display device
JP2005064189A
Green-emitting phosphor particle, method for manufacturing the green-emitting phosphor particle, color conversion sheet, light-emitting device, and image display device assembly
JP2011236310A
Fluorescent material particles, method for producing the same, and light emitting device
JP2017052927A
Phosphor, production method thereof, phosphor sheet and luminaire
JP2019026673A