Laminate and method for manufacturing laminate
The laminate with a low refractive index layer and gap structure addresses the issue of functional deterioration in optical functional layers, ensuring protection and maintaining light direction changing capabilities in decorative films.
Patent Information
- Application Number
- PCT/JP2024/003806
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-02-06
- Publication Date
- 2024-10-03
AI Technical Summary
Existing methods for protecting optical functional layers with convex surfaces, such as those used in decorative films, often result in functional deterioration when attempting to apply adhesives, leading to a loss of their light direction changing capabilities.
A laminate structure is developed with a low refractive index layer having a refractive index of 1.30 or less, directly contacting the convex surface of the optical functional layer and forming a gap between the two, which maintains the optical functionality while providing protection and mechanical strength.
The laminate effectively protects the optical functional layer, preventing functional deterioration and ensuring excellent transparency and mechanical strength, allowing for the maintenance of light direction changing capabilities.
Smart Images

Figure JP2024003806_03102024_PF_FP_ABST
Abstract
Description
Laminate and method for manufacturing the laminate
[0001] The present invention relates to a laminate and a method for manufacturing the laminate.
[0002] Decorative films are used as a means for improving the design of various products. For example, as disclosed in Patent Documents 1 and 2, depending on the application, decorative films may have an optical functional layer having a function of converting the direction of light. The optical functional layer having a function of converting the direction of light typically has a convex surface.
[0003] JP 2020-028981 A JP 2020-104467 A
[0004] If an attempt is made to protect the convex surface of the optical functional layer with, for example, an adhesive, the function of the optical functional layer may be reduced or lost.
[0005] The present invention has been made to solve the above-mentioned problems, and its main object is to provide a laminate that can protect an optical functional layer having a convex surface while suppressing deterioration of the function of the optical functional layer.
[0006] 1. A laminate according to an embodiment of the present invention comprises an optical functional layer having a first main surface and a second main surface facing each other, the optical functional layer having convex portions formed on the first main surface, and a low refractive index layer provided on the first main surface side of the optical functional layer and having a refractive index of 1.30 or less, wherein a gap is formed between the optical functional layer and the low refractive index layer. 2. In the laminate described in 1 above, the convex portions may have vertices. 3. In the laminate described in 1 or 2 above, the ratio of the height of the gap to the height of the convex portions may be 10% or more. 4. In the laminate described in any one of 1 to 3 above, the low refractive index layer may be in direct contact with the first main surface of the optical functional layer. 5. In the laminate described in any one of 1 to 4 above, the height of the convex portions may be 10 nm to 100 μm. 6. In the laminate described in any one of 1 to 5 above, the pitch of the convex portions may be 1 μm to 1000 μm. 7. In the laminate described in any one of 1 to 6 above, the low refractive index layer may be a porous layer composed of a porous body. 8. The laminate described in any one of the above 1 to 7 may have the optical functional layer, the low refractive index layer, and a first pressure-sensitive adhesive layer, in this order. 9. The laminate described in any one of the above 1 to 8 may have a second pressure-sensitive adhesive layer, the optical functional layer, and the low refractive index layer, in this order. 10. A method for producing a laminate according to an embodiment of the present invention includes preparing an optical functional layer having a first main surface and a second main surface facing each other, with convex portions formed on the first main surface, forming a coating film of a material that forms a low refractive index layer on the first main surface of the optical functional layer, and heating the coating film to form a low refractive index layer having a refractive index of 1.30 or less, wherein the heating forms a gap between the optical functional layer and the low refractive index layer.
[0007] According to the embodiment of the present invention, it is possible to protect the optical functional layer having a convex surface and to suppress deterioration of the function of the optical functional layer at the same time.
[0008] 1 is a schematic cross-sectional view illustrating an outline of a laminate according to an embodiment of the present invention, and is a diagram illustrating an optical functional layer included in the laminate shown in FIG.
[0009] Hereinafter, embodiments of the present invention will be described with reference to the drawings, but the present invention is not limited to these embodiments. In order to clarify the description, the drawings may schematically show the width, thickness, shape, etc. of each part compared to the embodiments, but these are merely examples and do not limit the interpretation of the present invention. Furthermore, in the drawings, the same or equivalent elements are given the same reference numerals, and redundant explanations may be omitted.
[0010] Fig. 1 is a schematic cross-sectional view showing the general configuration of a laminate according to one embodiment of the present invention, and Fig. 2 is a diagram illustrating an optical functional layer included in the laminate shown in Fig. 1. Note that, for ease of viewing, hatching of the optical functional layer is omitted in Figs. 1 and 2.
[0011] The laminate 100 includes an optical function layer 10 and a low-refractive index layer 20. The optical function layer 10 has a first main surface 10a and a second main surface 10b that face each other. The first main surface 10a is a convex surface, and the second main surface 10b is a flat surface. The optical function layer 10 is, for example, a lenticular lens configured with a plurality of linearly extending convex portions (e.g., cylindrical lenses) 11 arranged in parallel on a base 12. The convex portions 11 are arranged in the X direction (left-right direction) of FIG. 1, with their ridge lines directed in the Y direction in FIG. 1. The low-refractive index layer 20 is provided on the first main surface (convex surface) 10a side of the optical function layer 10.
[0012] The height H of the convex portion 11 of the optical function layer 10 1 The height H of the protrusion 11 can be set to any appropriate value. 1 is, for example, 10 nm to 100 μm, preferably 1 μm to 50 μm, more preferably 5 μm to 30 μm, and even more preferably 10 μm to 20 μm. In this specification, the "height of the convex portion" means the height from the bottom surface of the convex shape to the highest part (for example, the apex t).
[0013] The pitch P of the convex portions 11 of the optical function layer 10 can be set to any appropriate value. The pitch P of the convex portions 11 is, for example, 1 μm to 1000 μm, preferably 5 μm to 500 μm, more preferably 10 μm to 250 μm, and even more preferably 40 μm to 120 μm. In this specification, the "pitch of the convex portions" refers to the distance between the centers of adjacent convex portions in a planar view. In the illustrated example, the pitch P of the convex portions is the distance between the highest portions (e.g., vertices t) of adjacent convex portions 11. In one embodiment, the pitch P of the convex portions 11 substantially corresponds to the width D of the convex portions 11.
[0014] Height H of the substrate 12 of the optical function layer 10 2 can be set to any appropriate value. 2 is, for example, 15 μm to 360 μm, preferably 30 μm to 180 μm, and more preferably 60 μm to 120 μm.
[0015] The low-refractive index layer 20 is in direct contact with the first major surface 10a of the optical function layer 10. The low-refractive index layer 20 can be provided on the first major surface 10a via an adhesive layer (not shown), for example. However, providing the low-refractive index layer 20 directly on the first major surface 10a can avoid adverse effects caused by the refractive index of the adhesive layer, for example. The low-refractive index layer 20 can be directly formed on the optical function layer 10 by, for example, coating or printing a material for forming the low-refractive index layer. When the low-refractive index layer 20 is provided directly on the first major surface 10a of the optical function layer 10, the adhesive strength (e.g., 180° peel adhesive strength) of the low-refractive index layer 20 to the optical function layer 10 is preferably 1 N / 25 mm or more, more preferably 3 N / 25 mm or more, and even more preferably 5 N / 25 mm or more. The upper surface 20a of the low refractive index layer 20 may have an uneven shape following the unevenness of the convex surface 10a of the optical function layer 10, or may be a flat surface unlike the illustrated example.
[0016] In the laminate 100, a gap 13 is formed between the optical function layer 10 and the low-refractive index layer 20. The upper end 11a of the convex portion 11 of the optical function layer 10 is covered by the low-refractive index layer 20, and the gap 13 is formed by being surrounded by the convex portion 11 of the optical function layer 10 and the low-refractive index layer 20. In this way, by providing the low-refractive index layer 20 on the convex surface 10a side of the optical function layer 10 and forming the gap 13, the function of the optical function layer 10 can be maintained. For example, when the optical function layer 10 is a lenticular lens, the light collection area when parallel light is incident on the optical function layer 10 can be reduced. Furthermore, by providing the low-refractive index layer 20 on the convex surface 10a side of the optical function layer 10, a protective structure for the optical function layer 10 can be formed, and for example, mechanical strength can be ensured.
[0017] Height H of the protrusion 11 1 The height H of the gap 13 3 The ratio (H 3 ÷H 1 × 100, hereinafter referred to as the porosity) is, for example, greater than 0%, preferably 10% or more, more preferably 30% or more, even more preferably 40% or more, and particularly preferably 50% or more. Such a porosity allows the function of the optical function layer 10 to be maintained well. On the other hand, the porosity is, for example, less than 100%, preferably 90% or less, more preferably 80% or less, even more preferably 70% or less, and particularly preferably 60% or less. Such a porosity allows the optical function layer 10 to be well protected, and for example, excellent mechanical strength can be obtained.
[0018] The laminate 100 may have a first pressure-sensitive adhesive layer 31 provided on the first main surface 10a side of the optical functional layer 10. In the illustrated example, the first pressure-sensitive adhesive layer 31 is provided directly on the low refractive index layer 20. By providing the low refractive index layer 20, a protective structure can be formed by the first pressure-sensitive adhesive layer 31 while suppressing deterioration of the function of the optical functional layer 10 due to the first pressure-sensitive adhesive layer 31, and for example, mechanical strength can be ensured. Although not shown, the laminate 100 may have a second pressure-sensitive adhesive layer provided on the second main surface 10b side of the optical functional layer 10. In practice, it is preferable that a release liner (not shown) is temporarily attached to the surface of the pressure-sensitive adhesive layer until the laminate is used. Temporarily attaching the release liner protects the pressure-sensitive adhesive layer and enables the laminate to be rolled.
[0019] The optical functional layer typically has a light direction conversion function. A laminate including such an optical functional layer can achieve the following effects depending on the type of optical functional layer. For example, it can decorate the surface of various products to improve their design or aesthetic appeal. Specifically, (1) the color of the displayed image can be changed depending on the viewing angle; and / or (2) different images can be displayed depending on the viewing angle. Therefore, the laminate according to the embodiment of the present invention can also be referred to as a decorative film, optical laminate, etc. In the example shown in FIG. 1 , a decorative portion 40 is provided on the second main surface 10b of the optical functional layer 10. For example, the decorative portion 40 has a pattern corresponding to the size of the convex portion (e.g., a cylindrical lens) 11.
[0020] In addition to lenticular lenses, any suitable film having a textured surface can be used as the optical functional layer. Typical examples of the optical functional layer 10 include reflective hologram films, microlens array films, and prism films. The textured surface of the optical functional layer can be appropriately designed depending on the purpose. For example, any suitable textured surface that can exhibit functions such as light diffusion, light scattering, light reflection, and light diffraction can be used as the textured surface of a reflective hologram film. Typical examples include lenticular lenses as shown in the illustration, as well as Fourier transform structures, light diffraction patterns, and moth-eye structures. Furthermore, textured surfaces such as hairline patterns, matte patterns, line patterns, and interference patterns that do not have light diffraction functions but can exhibit unique brilliance can also be used. The dimensions of the convex and concave portions, such as the height and pitch of the convex portions, can be appropriately set depending on the textured surface.
[0021] The refractive index of the low refractive index layer 20 is typically 1.30 or less, with the lower limit exceeding 1.00. The refractive index of the low refractive index layer 20 is preferably 1.15 to 1.30, more preferably 1.17 to 1.28, even more preferably 1.18 to 1.26, and particularly preferably 1.19 to 1.24. With such a refractive index, deterioration in the function of the optical functional layer due to the provision of a layer on the first principal surface (convex surface) side of the optical functional layer can be extremely effectively suppressed. Unless otherwise specified, the refractive index refers to a refractive index measured at a wavelength of 550 nm. The refractive index is a value measured, for example, by the method described in the Examples below.
[0022] The total light transmittance of the low refractive index layer 20 is preferably 85% to 99%, more preferably 87% to 98%, and even more preferably 89% to 97%. By providing such a low refractive index layer on the first main surface (convex surface) of the optical functional layer, for example, it is possible to achieve excellent transparency for the entire laminate. As a result, for example, when the laminate is applied to various products, it is possible to ensure visibility of the product structure, images, etc. on the side opposite to the visible side of the optical functional layer. The total light transmittance can be measured, for example, using a haze meter described below.
[0023] The haze of the low refractive index layer 20 is preferably less than 5%, more preferably less than 3%. On the other hand, the haze may be, for example, 0.1% or more, or 0.2% or more. By providing such a low refractive index layer on the first main surface (convex surface) of the optical functional layer, for example, excellent transparency can be achieved for the entire laminate. As a result, for example, when the laminate is applied to various products, visibility of the product structure, image, etc. on the side opposite to the visible side of the optical functional layer can be ensured. The haze can be calculated, for example, from the following formula using values measured with a haze meter (for example, "HM-150" manufactured by Murakami Color Research Laboratory). Haze (%) = [Diffuse transmittance (%) / Total light transmittance (%)] × 100 (%)
[0024] The thickness of the low refractive index layer 20 is preferably 20 μm or less, more preferably 10 μm or less, even more preferably 8 μm or less, and may be 5 μm or less. With such a thickness, the function of the optical function layer 10 can be well maintained. On the other hand, the thickness of the low refractive index layer 20 is preferably 0.5 μm or more, more preferably 1 μm or more, even more preferably 1.5 μm or more, particularly preferably 2 μm or more, and most preferably 3 μm or more. With such a thickness, the optical function layer 10 can be well protected, and, for example, excellent mechanical strength can be obtained.
[0025] The low refractive index layer may have any suitable structure that can achieve the desired properties. Examples of materials that can be used for the low refractive index layer include those described in International Publication No. 2004 / 113966, Japanese Patent Application Laid-Open No. 2013-254183, and Japanese Patent Application Laid-Open No. 2012-189802. Representative examples of materials for the low refractive index layer include silicon compounds. Examples of silicon compounds include silica-based compounds; hydrolyzable silanes and their partial hydrolyzates and dehydration condensates; silicon compounds containing silanol groups; and activated silica obtained by contacting silicates with acids or ion exchange resins. Examples of materials for the low refractive index layer include organic polymers; polymerizable monomers (e.g., (meth)acrylic monomers and styrene-based monomers); and curable resins (e.g., (meth)acrylic resins, fluorine-containing resins, and urethane resins). These materials may be used alone or in combination.
[0026] In one embodiment, the low refractive index layer may contain spaces such as pores and gaps therein. In this case, the porosity of the low refractive index layer is preferably 20 vol% to 60 vol%, more preferably 25 vol% to 55 vol%, even more preferably 30 vol% to 50 vol%, and particularly preferably 35 vol% to 45 vol%. Such a porosity allows the refractive index of the low refractive index layer to be within an appropriate range and ensures strength. Here, the porosity is a value calculated using the Lorentz-Lorenz formula from the refractive index measured with an ellipsometer.
[0027] The size of the pores that can be contained in the low refractive index layer can be adjusted to a desired size depending on the purpose and application.The size of the pores that can be contained in the low refractive index layer is, for example, 2 nm or more, preferably 5 nm or more, more preferably 10 nm or more, and even more preferably 20 nm or more.On the other hand, the size of the pores that can be contained in the low refractive index layer is, for example, 500 nm or less, preferably 200 nm or less, and more preferably 100 nm or less.In addition, the size of the pores refers to the diameter of the major axis of the diameter of the major axis and the diameter of the minor axis of the pores.
[0028] The pore size can be quantified by the BET test method. In one embodiment, 0.1 g of a measurement sample (e.g., a formed low refractive index layer) is placed in the capillary of a specific surface area measurement device (e.g., "ASAP2020" manufactured by Micromeritics), and then dried under reduced pressure at room temperature for 24 hours to degas the gas contained in the measurement sample. Then, an adsorption isotherm is drawn by adsorbing nitrogen gas onto the measurement sample, and the pore size distribution is determined. This allows the pore size to be evaluated.
[0029] Examples of the low refractive index layer having a space therein include a porous layer made of a porous material and / or a layer containing an air layer at least in part. The low refractive index layer typically contains aerogel and / or particles (which may be hollow fine particles and / or porous particles, for example). The low refractive index layer is preferably a nanoporous layer (specifically, a layer in which 90% or more of the pores have a diameter of 10 -1 nm to 10 3 The thickness may be in the range of 100 nm.
[0030] Any appropriate particles may be used as the particles. The particles are typically composed of a silica-based compound. Examples of particle shapes include spherical, plate-like, needle-like, string-like, and bunch-of-grapes shapes. Examples of string-like particles include particles in which a plurality of spherical, plate-like, or needle-like particles are strung together like beads, short fiber-like particles (e.g., the short fiber-like particles described in JP 2001-188104 A), and combinations thereof. The string-like particles may be linear or branched. Examples of bunch-of-grapes-like particles include particles in which a plurality of spherical, plate-like, and needle-like particles are aggregated to form a bunch-of-grapes shape. The particle shape can be confirmed, for example, by observation with a transmission electron microscope.
[0031] An example of a low refractive index layer is a structure composed of one or more types of structural units that form a fine void structure, and these structural units are bonded together (for example, chemically bonded via catalytic action). Examples of the shape of the structural units include particulate, fibrous, rod-like, and flat-plate-like. The structural units may have only one shape, or may have a combination of two or more shapes.
[0032] A specific example of a low refractive index layer is a porous layer composed of a porous body in which particles having micropores (hereinafter referred to as micropore particles) are chemically bonded to each other. Such a porous layer can be obtained, for example, by chemically bonding the micropore particles to each other. The shape of the micropore particles is not particularly limited and may be, for example, spherical or other shapes. Furthermore, the micropore particles may be, for example, sol-gel beaded particles, nanoparticles (e.g., hollow nanosilica / nanoballoon particles), nanofibers, etc. Representative micropore particles include inorganic substances. Specific examples of inorganic substances include silicon (Si), magnesium (Mg), aluminum (Al), titanium (Ti), zinc (Zn), and zirconium (Zr). These may be used alone or in combination of two or more. In one embodiment, the micropore particles are, for example, micropore particles of a silicon compound, and the porous body is, for example, a silicone porous body. The micropore particles of the silicon compound include, for example, a pulverized gel silica compound.
[0033] Another example of a low refractive index layer is a layer containing a fibrous material such as nanofibers, in which spaces are formed by the entanglement of the fibrous material. Further examples of a low refractive index layer include a layer formed using hollow nanoparticles or nanoclay, or a layer formed using hollow nanoballoons or magnesium fluoride. The low refractive index layer may be composed of a single constituent material or multiple constituent materials. The low refractive index layer may be composed of a single form of the above examples, or multiple forms of the above examples.
[0034] The porous layer may have, for example, an open-cell structure in which the pores are interconnected. An open-cell structure refers to a porous body (e.g., a silicone porous body) in which the pores are interconnected three-dimensionally, and can also be described as a state in which the pore spaces are interconnected. The open-cell structure of the porous layer can increase the porosity. It is difficult to form an open-cell structure using closed-cell particles with individual pore structures, such as hollow particles (e.g., hollow silica). However, when using silica sol particles (a pulverized product of a gel-like silicon compound that forms a sol), the silica sol particles can have a three-dimensional dendritic structure, and the dendritic particles can settle and deposit in the coating film (a coating film of a sol containing a pulverized product of a gel-like silicon compound), thereby easily forming an open-cell structure. The porous layer preferably has a monolithic structure in which the open-cell structure includes a plurality of pore distributions. The monolithic structure refers to, for example, a hierarchical structure including a structure in which nano-sized fine pores exist and an open-cell structure in which nano-sized fine pores are aggregated. The monolithic structure, for example, can provide membrane strength through fine pores while providing high porosity through a coarse open-cell structure, thereby achieving both membrane strength and high porosity.
[0035] For example, the monolith structure can be formed by controlling the pore distribution of the void structure generated in the gel (gel silicon compound) before being crushed into silica sol particles.Also, for example, when crushing the gel silicon compound, the monolith structure can be formed by controlling the particle size distribution of the crushed silica sol particles to a predetermined size.In addition, the particle size distribution can be measured by, for example, a particle size distribution evaluation device such as dynamic light scattering method or laser diffraction method, or an electron microscope such as a scanning electron microscope (SEM) or a transmission electron microscope (TEM).
[0036] As described above, the porous layer may contain pulverized gel compounds such as gel silicon compounds, and the pulverized particles are chemically bonded (chemically bonded) to one another. The chemical bond is not particularly limited, and examples thereof include cross-linking, covalent bonding, and hydrogen bonding. The volume average particle size of the pulverized particles in the porous layer is, for example, 0.10 μm or more, preferably 0.20 μm or more, and more preferably 0.40 μm or more. Meanwhile, the volume average particle size of the pulverized particles in the porous layer is, for example, 2.00 μm or less, preferably 1.50 μm or less, and more preferably 1.00 μm or less. The volume average particle size is an index of the particle size variation of the pulverized particles and is determined by particle size distribution measurement.
[0037] The low refractive index layer may contain silicon atoms. For example, the silicon atoms contained in the low refractive index layer are preferably siloxane-bonded. Of all silicon atoms contained in the low refractive index layer, the proportion of unbonded silicon atoms (specifically, residual silanols) is, for example, less than 50%, preferably 30% or less, and more preferably 15% or less.
[0038] A laminate according to an embodiment of the present invention can be produced, for example, by preparing an optical functional layer having first and second principal surfaces facing each other and having a convex portion formed on the first principal surface, forming a coating film of a material for forming a low refractive index layer on the first principal surface (convex surface) of the optical functional layer, and heating the resulting coating film to form a low refractive index layer. By heating, the coating film can be unevenly distributed on the upper end side of the convex surface of the optical functional layer, and voids can be formed between the resulting low refractive index layer and the optical functional layer, as shown in FIG.
[0039] In one embodiment, the coating film can be formed using a coating liquid containing microporous particles, and the microporous particles can be chemically bonded to each other by heating (including drying) the coating liquid. The coating liquid containing microporous particles is, for example, a suspension. For example, a catalyst (crosslinking reaction accelerator) that promotes crosslinking between the microporous particles (e.g., a dehydration condensation reaction of residual silanol groups that may be contained in the microporous particles) and / or a substance that generates a catalyst (crosslinking reaction accelerator) (catalyst generator) may be added to the coating liquid. Examples of catalysts include photoactivated catalysts and thermally activated catalysts. Examples of catalyst-generating substances (catalyst generators) include photocatalyst generators and thermal catalyst generators. Examples of photocatalyst generators include photobase generators (catalysts that generate a basic catalyst upon light irradiation) and photoacid generators (substances that generate an acidic catalyst upon light irradiation). For example, the microporous particles are pulverized gel-like compounds (preferably gel-like silicon compounds), and the low refractive index layer is a porous layer composed of a porous body (preferably a silicone porous body) containing the pulverized gel-like compounds. Such microporous particles may have a state in which the three-dimensional structure of the gel-like compound before pulverization is dispersed in the three-dimensional basic structure, and by using such microporous particles, a structure based on the three-dimensional basic structure can be formed. Specifically, a new structure different from the three-dimensional structure of the gel-like compound can be formed. In this way, the finally obtained low refractive index layer (porous layer) may have a low refractive index similar to that of an air layer, for example. Furthermore, by chemically bonding the microporous particles to each other, the three-dimensional basic structure can be fixed, and sufficient strength can be ensured in the finally obtained low refractive index layer (porous layer). Details of the specific configuration and formation method of the low refractive index layer (porous layer) are described, for example, in International Publication No. 2019 / 151073. The description of this publication is incorporated herein by reference.
[0040] The coating thickness of the coating liquid can be set to a thickness that allows voids to be formed between the resulting low refractive index layer and the optical functional layer, and can be set appropriately depending on the size of the convex portions of the optical functional layer. For example, the coating thickness may be at least twice, at least 2.5 times, or at least 3 times the height of the convex portions. On the other hand, the coating thickness may be no more than 10 times the height of the convex portions. For example, the coating thickness may be at least 30 μm or at least 40 μm. On the other hand, the coating thickness may be no more than 200 μm. The heating temperature of the coating film (coating liquid) is, for example, 20° C. or higher, preferably 50° C. or higher. On the other hand, the heating temperature of the coating film (coating liquid) is, for example, 200° C. or lower, preferably 150° C. or lower. The heating time of the coating film (coating liquid) is, for example, 10 seconds or longer. On the other hand, the heating time of the coating film (coating liquid) is, for example, 24 hours or less, preferably 1 hour or less, more preferably 30 minutes or less, and even more preferably 10 minutes or less.
[0041] The pressure-sensitive adhesive layer is made of any appropriate pressure-sensitive adhesive. In one embodiment, the first pressure-sensitive adhesive layer 31 is made of a pressure-sensitive adhesive having a hardness that does not penetrate into spaces such as pores and gaps that may be contained in the low-refractive-index layer 20. The storage modulus of the first pressure-sensitive adhesive layer 31 at 23°C is typically 1.0 × 10 5 (Pa) ~1.0×10 7 (Pa). The storage modulus of the first pressure-sensitive adhesive layer 31 at 23° C. is, for example, 1.1×10 5 (Pa) or more, 1.2×10 5 (Pa) or more, 1.3×10 5 (Pa) or more, 1.4×10 5 (Pa) or more, 1.5×10 5 (Pa) or more, 1.6×10 5 (Pa) or more, 1.7×10 5 (Pa) or more, 1.8×10 5 (Pa) or more, 1.9×10 5 (Pa) or more or 2.0 x 10 5 (Pa) or more and 1.0 × 10 7 (Pa) or less, 5.0×10 6 (Pa) or less, 1.0×10 6 (Pa) or less or 5.0 x 105 The storage modulus of the first pressure-sensitive adhesive layer 31 at 23° C. is preferably 1.3×10 5 (Pa) ~1.0×10 6 (Pa), more preferably 1.5×10 5 (Pa) ~5.0×10 5 The storage modulus is determined by reading the value at 23°C when measured at a temperature rise rate of 5°C / min in the range of -50°C to 150°C under the condition of a frequency of 1 Hz in accordance with the method described in JIS K 7244-1 "Plastics - Test methods for dynamic mechanical properties."
[0042] A typical example of the adhesive constituting the first adhesive layer 31 is an acrylic adhesive (acrylic adhesive composition). The acrylic adhesive composition typically contains a (meth)acrylic polymer as the main component (base polymer). The (meth)acrylic polymer may be contained in the adhesive composition in a proportion of, for example, 50% by weight or more, preferably 70% by weight or more, and more preferably 90% by weight or more of the solid content of the adhesive composition. The (meth)acrylic polymer contains alkyl(meth)acrylate as a monomer unit as the main component. Note that (meth)acrylate refers to acrylate and / or methacrylate. Examples of the alkyl group of the alkyl(meth)acrylate include linear, branched, and other chain or cyclic alkyl groups having 1 to 20 carbon atoms. Examples of monomers constituting the (meth)acrylic polymer include, in addition to alkyl (meth)acrylates, comonomers such as carboxyl group-containing monomers, hydroxyl group-containing monomers, amide group-containing monomers, aromatic ring-containing (meth)acrylates, and heterocycle-containing (meth)acrylates.
[0043] The acrylic pressure-sensitive adhesive composition may contain an acrylic oligomer in addition to the base polymer (or a prepolymer, which is a partial polymer thereof). The acrylic oligomer may typically have a weight-average molecular weight of approximately 1,000 to 30,000. The acrylic oligomer contains alkyl (meth)acrylate as a monomer unit as a main component. For example, the acrylic pressure-sensitive adhesive composition is prepared by mixing the base polymer (prepolymer) with the acrylic oligomer, a silane coupling agent and / or a crosslinking agent, and other additives, as needed. The remaining monomers that can constitute the base polymer may be added to the acrylic pressure-sensitive adhesive composition as needed. Examples of the silane coupling agent include epoxy group-containing silane coupling agents. Examples of the crosslinking agent include isocyanate-based crosslinking agents and peroxide-based crosslinking agents.
[0044] The thickness of the first pressure-sensitive adhesive layer 31 is, for example, 3 μm to 60 μm, preferably 3 μm to 30 μm, and more preferably 5 μm to 10 μm. If the thickness of the first pressure-sensitive adhesive layer 31 is in this range, it has the advantage of having sufficient adhesive strength while having little effect on the optical function layer.
[0045] The present invention will be described in detail below using examples, but the present invention is not limited to these examples. The refractive index and storage modulus were measured as follows. Unless otherwise specified, "%" and "parts" in the examples are based on weight. <Refractive Index> A laminated film having a measurement target (e.g., a porous layer) formed on an acrylic film was cut to a size of 25 mm x 50 mm, and the resulting sample was attached to the surface of a glass plate (thickness: 3 mm) via an adhesive. The center of the back surface of the glass plate (approximately 20 mm in diameter) was filled in with black marker to prepare a sample that did not reflect light from the back surface of the glass plate. The obtained sample was placed in an ellipsometer (VASE, manufactured by J.A. Woollam Japan), and light with a wavelength of 550 nm was incident on the sample at an incident angle of 50 to 80 degrees to measure the refractive index. <Storage Modulus> A measurement target (e.g., an adhesive layer) was formed into a thickness of approximately 1.5 mm by lamination or other methods. This molded article was punched out into a disk shape with a diameter of 7.9 mm to prepare a test specimen. This test specimen was sandwiched between parallel plates, and viscoelasticity was measured under the following conditions using a dynamic viscoelasticity measuring device (Advanced Rheometric Expansion System (ARES) manufactured by Rheometric Scientific), to determine the storage modulus at 23°C. (Measurement conditions) Deformation mode: torsion Measurement frequency: 1 Hz Measurement temperature: -50°C to +150°C Heating rate: 5°C / min
[0046] [Manufacturing Example 1] Preparation of Coating Fluid for Forming Porous Layer (1) Gelation of Silicon Compound Mixture A was prepared by dissolving 0.95 g of methyltrimethoxysilane (MTMS), a precursor of the silicon compound, in 2.2 g of dimethyl sulfoxide (DMSO). 0.5 g of 0.01 mol / L oxalic acid solution was added to this mixture A, and the mixture was stirred at room temperature for 30 minutes to hydrolyze MTMS, producing a mixture B containing tris(hydroxy)methylsilane. 0.38 g of 28 wt% aqueous ammonia and 0.2 g of pure water were added to 5.5 g of DMSO, and then the mixture B was further added and stirred at room temperature for 15 minutes to gel the tris(hydroxy)methylsilane, thereby obtaining a mixture C containing a gel-like silicon compound. (2) Aging Treatment The mixture C containing the gel-like silicon compound prepared as above was incubated at 40 ° C. for 20 hours to undergo an aging treatment. (3) Pulverization Next, the gel-like silicon compound aged as described above was crushed into granules of several mm to several cm in size using a spatula. Next, 40 g of isopropyl alcohol (IPA) was added to the mixed solution C, and after light stirring, the mixture was left to stand at room temperature for 6 hours, and the solvent and catalyst in the gel were decanted. The same decantation process was performed three times to replace the solvent, yielding mixed solution D. The gel-like silicon compound in mixed solution D was then crushed (high-pressure media-less crushing). The crushing process (high-pressure media-less crushing) was performed using a homogenizer (manufactured by SMT Corporation, trade name "UH-50"), by weighing 1.85 g of the gel-like compound in mixed solution D and 1.15 g of IPA into a 5 cc screw bottle, and then crushing for 2 minutes under conditions of 50 W and 20 kHz. This crushing process crushed the gel-like silicon compound in mixed solution D, and mixed solution D became a crushed sol solution E. The volume average particle size, which indicates the particle size variation of the pulverized material contained in Sol E, was confirmed to be 0.50 to 0.70 μm using a dynamic light scattering Nanotrac particle size analyzer (manufactured by Nikkiso Co., Ltd., Model UPA-EX150).Furthermore, 0.062 g of a 1.5 wt % MEK (methyl ethyl ketone) solution of a photobase generator (Wako Pure Chemical Industries, Ltd., product name: WPBG266) and 0.036 g of a 5% MEK solution of bis(trimethoxysilyl)ethane were added to 0.75 g of sol solution E to obtain a coating liquid for forming a porous layer.
[0047] [Manufacturing Example 2-1] Pressure-Sensitive Adhesive Preparation 1 (Preparation of Acrylic Oligomer) 60 parts by weight of dicyclopentanyl methacrylate (DCPMA) and 40 parts by weight of methyl methacrylate (MMA) as monomer components, 3.5 parts by weight of α-thioglycerol as a chain transfer agent, and 100 parts by weight of toluene as a polymerization solvent were mixed and stirred at 70°C for 1 hour under a nitrogen atmosphere. Next, 0.2 parts by weight of 2,2'-azobisisobutyronitrile (AIBN) was added as a thermal polymerization initiator, and the mixture was reacted at 70°C for 2 hours, then heated to 80°C and reacted for 2 hours. The reaction solution was then heated to 130°C, and the toluene, chain transfer agent, and unreacted monomer were dried and removed to obtain a solid acrylic oligomer. The resulting acrylic oligomer had a weight-average molecular weight of 5100 and a glass transition temperature of 130°C.
[0048] (Preparation of Prepolymer) As monomer components for forming a prepolymer, 43 parts by weight of lauryl acrylate (LA), 44 parts by weight of 2-ethylhexyl acrylate (2EHA), 6 parts by weight of 4-hydroxybutyl acrylate (4HBA), and 7 parts by weight of N-vinyl-2-pyrrolidone (NVP) were blended, along with 0.015 parts by weight of "Omnirad 184" manufactured by IGM Resins as a photopolymerization initiator, and the mixture was irradiated with ultraviolet light to polymerize, thereby obtaining a prepolymer (polymerization rate: approximately 10%).
[0049] (Preparation of Pressure-Sensitive Adhesive Composition) To 100 parts by weight of the prepolymer, 0.07 parts by weight of 1,6-hexanediol diacrylate (HDDA), 3 parts by weight of the acrylic oligomer, and 0.3 parts by weight of a silane coupling agent ("KBM403" manufactured by Shin-Etsu Chemical Co., Ltd.) were added as post-addition components, and then these were mixed uniformly to prepare a pressure-sensitive adhesive composition.
[0050] (Formation of adhesive layer) A 75 μm thick polyethylene terephthalate (PET) film ("Diafoil MRF75" manufactured by Mitsubishi Chemical) having a silicone release layer on its surface was used as a substrate (double-duty release film), and the above-mentioned photocurable adhesive composition was applied to the substrate to a thickness of 50 μm to form a coating layer. Onto this coating layer, a 75 μm thick PET film ("Diafoil MRE75" manufactured by Mitsubishi Chemical) with one side treated with silicone release was attached as a cover sheet (double-duty release film). This laminate was then exposed from the cover sheet side to a lamp with an irradiation intensity of 5 mW / cm at the irradiated surface. 2 The adhesive was photocured by irradiating it with ultraviolet light using a black light whose position was adjusted so that the adhesive layer had a thickness of 50 μm.
[0051] [Production Example 2-2] Preparation of adhesive 2 (Preparation of acrylic adhesive solution) Into a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser, 90.7 parts of butyl acrylate, 6 parts of N-acryloylmorpholine, 3 parts of acrylic acid, 0.3 parts of 2-hydroxybutyl acrylate, and 0.1 parts by weight of 2,2'-azobisisobutyronitrile as a polymerization initiator were charged together with 100 g of ethyl acetate, and nitrogen gas was introduced while gently stirring to replace the atmosphere with nitrogen. Thereafter, a polymerization reaction was carried out for 8 hours while maintaining the liquid temperature in the flask at around 55°C, to prepare an acrylic polymer solution. An acrylic pressure-sensitive adhesive solution was prepared by blending 0.2 parts of an isocyanate crosslinking agent (Coronate L manufactured by Nippon Polyurethane Industry Co., Ltd., an adduct of trimethylolpropane and tolylene diisocyanate), 0.3 parts of benzoyl peroxide (Niper BMT manufactured by NOF Corporation), and 0.2 parts of γ-glycidoxypropylmethoxysilane (KBM-403 manufactured by Shin-Etsu Chemical Co., Ltd.) per 100 parts of the solid content of the obtained acrylic polymer solution.
[0052] (Formation of Pressure-Sensitive Adhesive Layer) Next, the acrylic pressure-sensitive adhesive solution was applied to one side of a silicone-treated polyethylene terephthalate (PET) film (manufactured by Mitsubishi Chemical Polyester Film Corporation, thickness: 38 μm) so that the thickness after drying (thickness of the pressure-sensitive adhesive layer formed) would be 10 μm, and the coating was dried at 150° C. for 3 minutes to form a pressure-sensitive adhesive layer. The storage modulus of the resulting pressure-sensitive adhesive was 1.3×10 5 (Pa).
[0053] [Example 1] A lenticular film (manufactured by Nippon Tokushu Kogaku Jushi Co., Ltd., "Lenticular Lens") having the shape shown in Figure 2 was used as the optical functional layer. The height H of the convex portion of the lenticular film 1 is 17 μm, the width D of the convex portions (the pitch P of the convex portions) is 80 μm, and the height H of the base 2 The thickness was 95 μm. The porous layer-forming coating solution prepared in Production Example 1 was applied to the convex surface of this lenticular film to a coating thickness of 50 μm to 60 μm, resulting in a coating film. The coating film was then dried by heating at 100°C for 1 minute to form a porous body. The dried porous body was irradiated with ultraviolet light. Specifically, the dried porous body was irradiated with light having a wavelength of 360 nm at a light irradiation dose (energy) of 500 mJ. A pressure-sensitive adhesive layer (50 μm thick) composed of the pressure-sensitive adhesive prepared in Production Example 2-1 was then bonded to the surface of the porous body, and heat aging was performed at 60°C for 22 hours to form a porous layer on the lenticular film. In this way, a laminate having a configuration of lenticular film / porous layer / first pressure-sensitive adhesive layer was produced. The refractive index of the resulting porous layer was 1.15, and the porosity was 60%. By heating (drying), the coating film was unevenly distributed on the upper end side of the convex portions of the lenticular film, and voids were formed between the convex surfaces of the lenticular film and the porous body, as shown in Figure 1. The maximum thickness of the resulting porous layer was 6 μm, and the height of the voids H 3 The thickness was 10 μm and the porosity was 59%.
[0054] [Comparative Example 1] A laminate was produced in the same manner as in Example 1, except that the coating thickness in the coating of the porous layer-forming coating liquid was changed to less than 30 μm. Note that, by heating (drying) the coating film, no voids were formed between the convex surfaces of the lenticular film and the porous body (the finally obtained porous layer was formed so as to fill the spaces between the convex portions of the lenticular film), as shown in Fig. 1 ), and the maximum thickness of the obtained porous layer was 1.4 μm, and the porosity was 0%.
[0055] [Comparative Example 2] A laminate was produced in the same manner as in Example 1, except that a first pressure-sensitive adhesive layer was directly formed on the convex surface of the optical functional layer (a porous layer was not formed by applying a coating liquid for forming a porous layer without heating or irradiating with ultraviolet light) and that heat aging was not performed. In the obtained laminate, the first pressure-sensitive adhesive layer was embedded between the convex portions of the lenticular film, and no gaps were formed between the convex surfaces of the lenticular film and the first pressure-sensitive adhesive layer.
[0056] [Comparative Example 3] A laminate was produced in the same manner as in Example 1, except that a first pressure-sensitive adhesive layer was directly formed on the convex surface of the optical functional layer (a porous layer-forming coating liquid was applied without heating or ultraviolet irradiation to form a porous layer), and that the pressure-sensitive adhesive prepared in Production Example 2-2 was used as the pressure-sensitive adhesive constituting the first pressure-sensitive adhesive layer, and heat aging was not performed. In the obtained laminate, the first pressure-sensitive adhesive layer did not enter between the convex portions of the lenticular film, and gaps were formed between the convex surfaces of the lenticular film and the first pressure-sensitive adhesive layer.
[0057] [Evaluation] The laminates obtained in the Examples and Comparative Examples were evaluated as follows. The evaluation results are shown in Table 1. (1) Optical Properties A pattern was prepared on which 40 μm-wide thin lines in different colors (two colors) corresponding to the size of the convex portions of the lenticular film were printed, with the lines arranged alternately without gaps. The resulting laminate was placed on this pattern, and the pattern was observed from the surface of the laminate. Specifically, the change in the pattern visible when the viewing angle relative to the laminate surface was changed was evaluated. The evaluation criteria were as follows: (Evaluation Criteria) ○ (Good): The pattern changed when observed at different angles, and was observable from any angle × (Poor): The pattern did not change when observed at different angles (2) Mechanical Strength The mechanical strength was evaluated by a peel test. For the peel test, a pressure-sensitive adhesive sheet in which a pressure-sensitive adhesive layer was laminated on a PET film measuring 25 mm wide x 300 mm long was used in the lamination of the pressure-sensitive adhesive layer in the production of the laminates of the Examples and Comparative Examples, and a test sample (laminate) measuring 25 mm wide x 300 mm long was obtained. The obtained test samples were subjected to a 180° peel test using a tensile tester (manufactured by Minebea Co., Ltd., product name: TCM-1kNB) in which the porous layer or the first pressure-sensitive adhesive layer was peeled off in the lengthwise direction from the lenticular film (optical functional layer) of the laminate, and the interlayer adhesive strength (180° peel adhesive strength) (unit: N / 25 mm) between the optical functional layer and the adjacent layer was measured. The measurement was performed in an atmosphere of 23°C and 50% RH, at a peel angle of 180° and a pulling rate of 300 mm / min. The evaluation criteria were as follows: (Evaluation Criteria) ◎ (Very good): Adhesion strength of 5 N / 25 mm or more ○ (Good): Adhesion strength of 1 N / 25 mm or more but less than 5 N / 25 mm × (Poor): Adhesion strength of less than 1 N / 25 mm
[0058]
[0059] As is clear from Table 1, according to the examples of the present invention, it is possible to ensure mechanical strength while maintaining the function of the optical functional layer.
[0060] The laminate according to the embodiment of the present invention can be suitably used, for example, as a decorative film.
[0061] REFERENCE SIGNS LIST 10 Optical functional layer 10a First main surface (convex surface) 10b Second main surface 11 Convex portion 12 Base 13 Void 20 Low refractive index layer 31 First pressure-sensitive adhesive layer 100 Laminate
Claims
1. A laminate comprising: an optical functional layer having a first principal surface and a second principal surface opposed to each other, with a convex portion formed on the first principal surface; and a low refractive index layer having a refractive index of 1.30 or less, provided on the first principal surface side of the optical functional layer, wherein a gap is formed between the optical functional layer and the low refractive index layer.
2. The laminate according to claim 1, wherein the protrusion has an apex.
3. The laminate according to claim 1, wherein the ratio of the height of said gaps to the height of said protrusions is 10% or more.
4. The laminate according to claim 1, wherein the low refractive index layer is in direct contact with the first main surface of the optically functional layer.
5. The laminate according to claim 1, wherein the height of the protrusions is from 10 nm to 100 μm.
6. The laminate according to claim 1, wherein the pitch of the protrusions is 1 μm to 1000 μm.
7. The laminate according to claim 1, wherein the low refractive index layer is a porous layer made of a porous body.
8. The laminate according to claim 1, comprising the optically functional layer, the low refractive index layer, and a first pressure-sensitive adhesive layer in this order.
9. The laminate according to claim 1, comprising a second pressure-sensitive adhesive layer, the optically functional layer, and the low refractive index layer in this order.
10. A method for manufacturing a laminate, comprising: preparing an optical functional layer having first and second main surfaces opposing each other, with a convex portion formed on the first main surface; forming a coating film of a material that forms a low refractive index layer on the first main surface of the optical functional layer; and heating the coating film to form a low refractive index layer having a refractive index of 1.30 or less, wherein the heating forms a gap between the optical functional layer and the low refractive index layer.
Citation Information
Patent Citations
Antireflection film, polarizing plate and image display device
JP2001188104A
Antireflection film, polarizer and display device
JP2012189802A
Antireflection film, manufacturing method thereof, polarizer, and image display device
JP2013254183A
Decoration film and method for producing the same
JP2020028981A
Decorative film
JP2020104467A