Coated active material particles, active material layer, and lithium ion secondary battery

Coated active material particles with phosphorus-containing lithium compounds address the issue of gas generation in lithium ion secondary batteries by stabilizing the electrolyte and enhancing ion conductivity, improving battery performance and stability.

WO2024202644A1PCT designated stage expired Publication Date: 2024-10-03KANEKA CORP

Patent Information

Application Number
PCT/JP2024/005190
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-07
Filing Date
2024-02-15
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Lithium ion secondary batteries face issues with gas generation due to electrolyte decomposition, particularly in non-aqueous electrolyte systems using lithium nickel manganese oxide (LNMO) as the positive electrode active material, leading to instability and performance degradation.

Method used

Coated active material particles with a film comprising phosphorus-containing lithium compounds, including phosphate ions and metal species like Fe, Mn, and Si, are used to suppress gas generation by forming a shell film and buffer layer on the active material particles, enhancing the electrolyte's stability and ion conductivity.

Benefits of technology

The coated active material particles effectively reduce gas generation during electrolyte decomposition, ensuring better stability and performance of lithium ion secondary batteries by maintaining a stable electrolyte environment and facilitating smooth ion transfer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024005190_03102024_PF_FP_ABST
    Figure JP2024005190_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides: coated active material particles with which it is possible to suppress the generation of a gas due to decomposition of an electrolyte solution; an active material layer; and a lithium ion secondary battery. The coated active material particles are obtained by covering active material particles with a coating film, the coating film comprising a phosphate ion-containing lithium compound that contains lithium ions, a metal species, and phosphate ions.
Need to check novelty before this filing date? Find Prior Art

Description

Coated active material particles, active material layer, and lithium ion secondary battery

[0001] The present invention relates to coated active material particles, an active material layer, and a lithium ion secondary battery.

[0002] BACKGROUND ART Lithium nickel manganese oxide (hereinafter also referred to as LNMO) has been known as a positive electrode active material for lithium ion secondary batteries (for example, see Patent Document 1).

[0003] LNMO has an operating voltage of 4.7 V based on the lithium metal deposition potential, which is higher than that of conventional lithium insertion materials used as positive electrode active materials (for example, lithium cobalt oxide, which has a voltage of 4 V), and is therefore expected to contribute to achieving higher energy density.

[0004] Japanese Patent Application Laid-Open No. 2021-051987

[0005] Incidentally, in lithium ion secondary batteries, the crystal structure of the active material changes when Li ions are inserted and extracted, and distortion occurs within the crystal structure, which can cause instability.

[0006] In such cases, transition metal ions constituting the crystalline structure of the positive electrode active material are eluted, and in the vicinity of the positive electrode, the bond between the transition metal and oxygen is broken, causing oxygen to be released, resulting in the generation of oxygen gas, or the generation of carbon dioxide gas by reaction with the electrolytic medium. In particular, in a lithium ion secondary battery using a nonaqueous electrolyte as the electrolytic medium and LNMO as the positive electrode active material, the operating voltage is high and the reaction proceeds in an oxidizing atmosphere near the positive electrode, which causes the problem of the above-mentioned gas generation becoming more pronounced.

[0007] Furthermore, in the vicinity of the negative electrode, there is a problem that the electrolytic medium is reduced due to a change in the crystal structure caused by the insertion and desorption of Li ions into and from the negative electrode active material, resulting in the generation of hydrogen gas and the like.

[0008] Thus, in lithium ion secondary batteries, it is required to suppress the generation of these gases.

[0009] Therefore, an object of the present invention is to provide coated active material particles, an active material layer, and a lithium ion secondary battery that can suppress gas generation due to decomposition of an electrolytic medium compared to conventional techniques.

[0010] One aspect of the present invention for solving the above-mentioned problems is coated active material particles in which active material particles are coated with a coating, and the coating contains a phosphate ion-containing lithium compound that contains lithium ions, a metal species, and phosphate ions.

[0011] The term "metal species" as used herein refers to chemical species of metals, and is a concept that includes ions, atoms, atomic groups, elements, and compounds. The term "metal" as used herein also includes silicon.

[0012] According to this aspect, when the active material is used as an electrode for a lithium-ion secondary battery that uses an electrolyte solution as an electrolytic medium, the coating that covers the active material particles contains a phosphate ion-containing lithium compound, thereby suppressing the generation of gas due to decomposition of the electrolyte solution.

[0013] In a preferred aspect, the phosphate ion-containing lithium compound contains elemental manganese.

[0014] In a preferred aspect, the phosphate ion-containing lithium compound contains a silicon element.

[0015] In a preferred aspect, the two surfaces of the coating differ in at least one of the concentration of the phosphate ions, the concentration of the metal species, and the composition.

[0016] The term "different in composition" as used herein includes not only different composition ratios of constituent elements but also different types of constituent elements. The same applies hereinafter.

[0017] A preferred aspect includes core-shell particles having a core-shell structure in which the active material particles form a core and a continuous shell film forms the shell, the shell film forms the outer surface of the core-shell particle, the coating has the shell film and a buffer portion in this order from the active material particle side, the buffer portion is formed and distributed on the outer surface of the shell film, and the coating differs on both sides of the shell film in at least one of the concentration of the phosphate ions, the concentration of the metal species, and composition.

[0018] In a preferred aspect, the coating differs in at least one of the concentration of the phosphate ions, the concentration of the metal species, and the composition on both sides of the buffer portion.

[0019] In a preferred aspect, the average occupancy rate of the buffer portion relative to the outer surface of the shell film per active material particle is 0.1% or more and 30% or less.

[0020] In a preferred aspect, the phosphate ion-containing lithium compound has an olivine-type crystal structure.

[0021] One aspect of the present invention is an active material layer including the above-described coated active material particles, wherein the coating has a shell film in contact with the active material particles, the shell film contains the phosphate ion-containing lithium compound, the phosphate ion-containing lithium compound contains one or more metals selected from the group consisting of Fe, Mn, Si, and Al, and the cross-sectional shape of the active material layer is a sea-island structure having island portions and a sea-like portion, the island portions including a permeable pore network, and the sea-like portion including the active material particles, a binder, and a conductive network.

[0022] According to this aspect, since the shell film contains a phosphate ion-containing lithium compound containing one or more metals selected from the group consisting of Fe, Mn, Si, and Al, when used as an electrode for a lithium-ion secondary battery using an electrolyte solution as an electrolytic medium, it is possible to suppress the generation of gas due to decomposition of the electrolyte solution caused by direct exposure of the active material particles to the electrolyte solution. According to this aspect, since the active material has a conductive network and a permeable pore network, when used as an electrode for a lithium-ion secondary battery, the exchange of charges and lithium ions between the electrolyte solution and the active material particles is facilitated, and the electrode reaction is likely to occur.

[0023] In a preferred aspect, the conductive network is at least partially in contact with the active material particles or the shell film, the permeable pore network has pores and is at least partially in contact with the active material particles or the shell film, and the permeable pore network has a lithium ion conductor extending from the contact portion with the active material particles or the shell film toward the pores.

[0024] In a preferred aspect, the active material particles are negative electrode active material particles for a lithium ion secondary battery and contain lithium titanate.

[0025] In a preferred aspect, the active material particles are positive electrode active material particles for a lithium ion secondary battery and contain lithium nickel manganese oxide.

[0026] One aspect of the present invention is an active material layer containing active material particles for a lithium ion secondary battery, the active material layer having a cross-sectional shape of a sea-island structure, with island-like portions and a sea-like portion, the island-like portions including a permeable pore network, and the sea-like portion including the active material particles, a binder, and a conductive network.

[0027] According to this aspect, when the active material is used as an electrode for a lithium ion secondary battery that uses an electrolyte solution as an electrolytic medium, it is possible to suppress gas generation due to decomposition of the electrolyte solution. According to this aspect, an active material layer for a high-capacity lithium ion secondary battery that has excellent conductivity of electrons and Li ions and achieves uniform potential is obtained.

[0028] In a preferred aspect, the active material particles are coated active material particles coated with a coating film, the coating film is a multilayer film including at least two layers, a shell film and a buffer portion, from the active material particle side, the conductive network is made of a conductive material and has a conductive network cell contact portion in contact with the shell film, and the permeable pore network has a pore shell contact portion in contact with the shell film via the buffer portion.

[0029] In a preferred aspect, the buffer portion is formed from the pore-shell contact portion to the conductive network, and the conductive network-cell contact portion is held between two adjacent pore-shell contact portions on the surface of the active material particle.

[0030] A preferred embodiment has a silicon-containing compound film containing elemental silicon.

[0031] In a preferred aspect, the buffer portion has a non-liquid lithium ion conductor having a solid electrolyte interface (SEI) structure, and the lithium ion conductor is disposed in the pore-shell contact portion.

[0032] In a preferred aspect, the shell film is a phosphate ion-containing lithium compound containing one or more metals selected from the group consisting of Fe, Mn, Si, and Al.

[0033] One aspect of the present invention is a lithium ion secondary battery in which an electrode stack having a positive electrode and a negative electrode facing each other with an electrolyte sandwiched therebetween is enclosed within an outer casing, and the positive electrode or the negative electrode contains the above-mentioned coated active material particles.

[0034] According to this aspect, it is possible to suppress the generation of gas due to decomposition of the electrolyte solution, which is the electrolytic medium.

[0035] One aspect of the present invention is coated active material particles in which active material particles are coated with a coating, the coating containing a metal component (wherein silicon element is included as the metal) and a phosphate ion-containing lithium compound containing phosphate ions, and the concentrations of the phosphate ions differ on both sides of the coating.

[0036] One aspect of the present invention is coated active material particles in which active material particles are coated with a coating, the coating containing a metal component (including silicon element as the metal) and a phosphate ion-containing lithium compound containing phosphate ions, and the components and / or compositions of the metal differ on both sides of the coating.

[0037] The above aspects may be made dependent on each other, or some of the configurations may be quoted or substituted for each other, as long as they are included in the technical scope of the present invention.

[0038] According to the coated active material particles, active material layer, and lithium ion secondary battery of the present invention, gas generation due to decomposition of the electrolytic medium can be suppressed compared to conventional techniques.

[0039] 1A is a cross-sectional view of the positive electrode part and the negative electrode part of FIG. 1B is a cross-sectional view of the electrode part, and FIG. 1C is a cross-sectional view of the coated active material particle.

[0040] Hereinafter, embodiments of the present invention will be described in detail.

[0041] As shown in Fig. 1 , a lithium ion secondary battery (also simply referred to as LIB) 1 according to a first embodiment of the present invention has a battery assembly 2 in which an electrode stack 5 is housed within an outer casing 3, and the outer casing 3 of the battery assembly 2 is filled with an electrolytic medium 6 and sealed. In the lithium ion secondary battery 1, the electrolytic medium 6 may be a nonaqueous electrolyte LIB, an all-solid-state LIB having a solid electrolyte, or a polymer LIB having a polymer electrolyte, with the nonaqueous electrolyte LIB being preferred. In the following description, the lithium ion secondary battery 1 will be described as being a battery with a nonaqueous electrolyte LIB.

[0042] <Exterior Body 3> The exterior body 3 is not particularly limited as long as it has an internal space, can accommodate and seal the electrode stack 5 and the electrolytic medium 6 in the internal space, is chemically stable against the electrolytic medium 6, and has water vapor barrier properties. For example, the exterior body 3 can be a can made primarily of aluminum, iron, or stainless steel, or a laminate film containing a laminate resin.

[0043] <Electrode Stack 5> As shown in FIG. 1, the electrode stack 5 has a positive electrode part 10, a negative electrode part 11, a separator 12, a positive electrode take-out member 13, and a negative electrode take-out member 14.

[0044] (Positive electrode section 10) As shown in Fig. 1(b), the positive electrode section 10 is an intercalation electrode in which a positive electrode active material layer 21 is laminated on at least one main surface of a positive electrode current collector 20, and Li ions can be inserted and extracted. As shown in Fig. 2(a), the positive electrode section 10 of this embodiment has positive electrode active material layers 21 laminated on both main surfaces of the positive electrode current collector 20.

[0045] 1(c), the negative electrode part 11 is an intercalation electrode in which a negative electrode active material layer 121 is laminated on at least one main surface of a negative electrode current collector 120, and in which the negative electrode active material layer 121 is laminated on the negative electrode current collector 120. The negative electrode part 11 is an intercalation electrode in which Li ions can be inserted and extracted, similar to the positive electrode part 10 shown in FIG.

[0046] (Current collectors 20, 120) The current collectors 20, 120 are electrically conductive plate-like or film-like bodies, and are not particularly limited as long as they are electrically conductive. For example, aluminum or an aluminum alloy can be used for the current collectors 20, 120. However, aluminum or an aluminum alloy is preferred because it is stable in a reactive atmosphere, and a coated body in which a metal surface is coated with a metal that does not react at the potential of the positive or negative electrode can be used.

[0047] (Active material layer 21, 121) The active material layer 21, 121 is a Li ion conductive active material and has a plurality of coated active material particles 30, 130, binders 70, 70, conductive networks 80, 80, and permeable pore networks 81, 81, as shown in the enlarged view of FIG. 2( a). The active material layer 21, 121 preferably has an SEI (Solid Electrolyte Interphase) structure. As shown in the enlarged view of FIG. 2( a), the active material layer 21, 121 is a sea-island film having a sea-island structure, and is a bulk film whose cross-sectional shape includes island-like portions 60 and sea-like portions 61.

[0048] The active material layers 21, 121 are largely occupied by the coated active material particles 30, 130 in terms of weight ratio, but the binder 70 and the conductive network 80 occupy a large proportion in terms of volume ratio, to the extent that they can be confirmed even with an electron microscope.

[0049] 2(b), the coated active material particle 30 includes a core-shell particle 36 having a core-shell structure in which the positive electrode active material particle 40 serves as a core and the shell film 41 serves as a shell. That is, in the core-shell particle 36, the outer surface of the positive electrode active material particle 40 is covered with the shell film 41.

[0050] Furthermore, the coated active material particle 30 of this embodiment further includes a buffer portion 42 on a part or all of the outer surface of the shell film 41. That is, in the coated active material particle 30 of this embodiment, the surface of the positive electrode active material particle 40 is covered with a coating 35, and the coating 35 is a multilayer film of the shell film 41 and the buffer portion 42.

[0051] The coated active material particle 130 includes a core-shell particle 136 having a core-shell structure with the negative electrode active material particle 140 as the core and the shell film 41 as the shell. That is, in the core-shell particle 136, the outer surface of the negative electrode active material particle 140 is covered with the shell film 41. The coated active material particle 130 of this embodiment further includes a buffer portion 42 on part or all of the outer surface of the shell film 41. The shell film 41 and buffer portion 42 of the coated active material particle 130 are similar to the shell film 41 and buffer portion 42 of the coated active material particle 30, but the negative electrode active material particle 140 serving as the core is different from the coated active material particle 30. That is, in the coated active material particle 130 of this embodiment, the surface of the negative electrode active material particle 140 is covered with a coating 35, and the coating 35 is a multilayer film including the shell film 41 and the buffer portion 42.

[0052] Here, it is preferable that the relative Li ion content of the shell film 41 of the coated active material particle 130 constituting the negative electrode active material layer 121 is different from the relative Li ion content of the shell film 41 of the coated active material particle 30 constituting the positive electrode active material layer 21.

[0053] The positive electrode shell film Li ion concentration, which is the concentration of Li ions contained in the shell film 41 of the coated active material particle 30, is preferably different from the negative electrode shell film Li ion concentration, which is the concentration of Li ions contained in the shell film 41 of the negative electrode active material particle 140. Note that the positive electrode shell film Li ion concentration and the negative electrode shell film Li ion concentration are average concentrations in the film.

[0054] (Active material particles 40, 140) The positive electrode active material particles 40 are lithium transition metal composite oxide particles, and are capable of inserting and extracting Li ions. The positive electrode active material particles 40 have an average potential of the desorption and insertion of Li ions relative to the deposition potential of lithium metal (vs. Li + / Li), is preferably 4.5 V or more and 5.0 V or less. That is, the positive electrode active material particles 40 preferably have an operating potential of 4.5 V or more and 5.0 V or less relative to lithium metal. + / Li) can be obtained by, for example, measuring the charge / discharge characteristics of a half cell with a working electrode using the positive electrode active material particles 40 and a lithium metal counter electrode, and reading the voltage values ​​at the start and end of the plateau. When there are two or more plateaus, the plateau with the lowest voltage value is 4.5 V (vs. Li + / Li) or more, and the highest voltage plateau is 5.0 V (vs. Li + / Li) or less.

[0055] The positive electrode active material particles 40 are not particularly limited, but are preferably a spinel-type lithium manganese oxide represented by the following formula (1): Li 1+x M y Mn 2-x-y O 4 In the formula (1), x and y satisfy 0≦x≦0.2 and 0<y≦0.8, respectively, and M is at least one element selected from the group consisting of Al, Mg, Zn, Ni, Co, Fe, Ti, Cu, and Cr.

[0056] Among the compounds represented by formula (1), lithium nickel manganese oxide (LNMO) in which M is Ni is preferred.

[0057] From the viewpoint of reducing lithium deposition and improving safety, it is preferable to use lithium titanate for the negative electrode active material particles 140. Among lithium titanates, lithium titanate with a spinel structure is particularly preferable for the negative electrode active material particles 140 from the viewpoint of small expansion and contraction of the active material during the Li ion insertion and desorption reactions. The lithium titanate may contain trace amounts of elements other than lithium and titanium, such as Nb.

[0058] The particle size of the active material particles 40, 140 is not particularly limited, but the median diameter d50 is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 20 μm or more. The positive electrode active material particles 40, 140 preferably have a median diameter d50 of 100 μm or less, more preferably 80 μm or less, even more preferably 50 μm or less, and particularly preferably 30 μm or less.

[0059] (Shell film 41) The shell film 41 is a film having a continuous layer structure that densely covers the surface shape of the active material particle 40, 140, and is a coating made of a Li ion conductive oxide containing phosphorus as an element. The shell film 41 that constitutes the coated active material particle 30 is preferably made of an intercalation material that functions alone as a positive electrode active material.

[0060] Shell film 41 contains a phosphate ion-containing lithium compound that contains phosphate ions and one or more metals (metal species) selected from the group consisting of Fe, Mn, Si, and Al. The phosphate ion-containing lithium compound is preferably a lithium phosphate compound such as lithium manganese phosphate (hereinafter also referred to as LMP) or lithium iron phosphate (hereinafter also referred to as LFP) having an olivine-type crystal structure, lithium titanium aluminum phosphate (hereinafter also referred to as LATP) or lithium phosphate (hereinafter also referred to as LP) having a NASICON-type crystal structure, and more preferably a lithium transition metal phosphate such as LMP, LFP, or LATP.

[0061] Among these, it is more preferable that shell film 41 be LMP, which is a phosphate ion-containing lithium compound film containing manganese (Mn) element.

[0062] The shell film 41 preferably has a two-layer structure of LFP / LMP, with different metals and / or compositions on both sides, from the center to the outside of the active material particle 40, 140. It is more preferable that the transition metal constituting the shell film 41 gradually changes from Fe to Mn. It is even more preferable that the shell film 41, together with the buffer portion 42, change the composition and / or ratio of the metals in the Li-based polyanion.

[0063] The thickness of shell film 41 is thinner than the particle diameter of the Li ion conductive oxide, and is preferably 5 nm to 20 nm, more preferably 5 nm to 15 nm, inclusive. Within this range, the amount of gas generation can be suppressed while suppressing resistance loss in shell film 41.

[0064] Shell film 41 covers at least a portion, more preferably 95% or more, and preferably completely covers the surface of active material particles 40, 140. Shell film 41 is preferably amorphous from the viewpoint of replenishing Li ions in active material particles 40, 140 that have been consumed by the SEI structure of buffer section 42, which will be described later.

[0065] (Buffer Section 42) The buffer section 42 is a silicon-containing compound film containing lithium and silicon. The buffer section 42 has a solid electrolyte interface (hereinafter also referred to as SEI) structure formed by an electrochemical reaction between the core-shell particles 36 and the interface electrolyte, and is a siloxane-modified coating layer containing silicon. The buffer section 42 is a selectively permeable membrane that allows only Li ions to pass through but not electrons. The buffer section 42 is an insertion / destruction prevention layer that prevents destruction of the structure of the core-shell particles 36, 136 by inserting organic solvent molecules with large molecular weights that move with Li ions in the electrolytic medium 6 into the core-shell particles 36, particularly into the Li ion insertion / desorption sites of the active material particles 40, 140. The buffer section 42 preferably includes a modified region integral with the SEI structure on the surface near the interface with the core-shell particles 36, 136, particularly at the contact area with the permeable pore network 81. The buffer portion 42 may contain, in addition to lithium and silicon elements, a metal oxide and / or a metal phosphate.

[0066] The shell film 41 / buffer section 42 multilayer preferably has different concentrations and / or compositions of metal species (metal ions) and different concentrations of phosphate ions on both sides. The shell film 41 / buffer section 42 multilayer preferably has a decreased phosphate ion concentration and an increased oxide concentration from the center to the periphery of the active material particle 40, 140. In the shell film 41 / buffer section 42 multilayer, the shell film 41 preferably contains LMP. The shell film 41 / buffer section 42 multilayer preferably has a gradually varying composition and / or concentration.

[0067] The buffer sections 42 cover at least a portion of the surface of the core-shell particles 36, 136. The buffer sections 42 are distributed on the outer surface of the shell film 41, and it is preferable that the coating 35 differs between both surfaces of the shell film 41 in at least one of the concentration of phosphate ions, the concentration of metal species, and the composition. It is preferable that the average occupation rate of the buffer sections 42 relative to the outer surface of the shell film 41 per active material particle 40, 140 is 0.1% or more and 30% or less.

[0068] (Binder 70) The binder 70 is not particularly limited, but may be at least one selected from the group consisting of polyethylene glycol (PEG), polyethylene oxide (PEO), polyacrylonitrile (PAN), polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), styrene-butadiene rubber, polyimide, and derivatives thereof. The binder 70 may also contain a dispersant, a thickener, and a conductive additive that dissolves in the binder material. The amount of binder 70 is preferably 1 part by weight to 30 parts by weight per 100 parts by weight of the core-shell particles 36, 136. Within this range, the active material layer 21, 121 can be formed in which the core-shell particles 36, 136 are bonded with sufficient adhesive strength, and a stable, low-resistance conductive network 80 can be constructed. Furthermore, sufficient adhesive strength can be obtained with the current collector 20, 120. Furthermore, the active material layer 21, 121 can be given the strength to support the active material particles 40, 140 and the core-shell particles 36, 136 as an integral layer, a stable low-resistance conductive network 80 can be formed, and sufficient adhesive strength with the current collector 20, 120 can be achieved.

[0069] (Conductive Network 80) The conductive network 80 is composed of a conductive material such as a conductive additive, preferably a conductive carbon material, and more preferably at least one selected from natural graphite, artificial graphite, vapor-grown carbon fiber, carbon nanotubes, acetylene black, ketjen black, and furnace black. The amount of the conductive material constituting the conductive network 80 contained in the active material layer 21, 121 is preferably 1 part by weight to 30 parts by weight per 100 parts by weight of the core-shell particles 36, 136. This range ensures the conductivity of the electrode unit 10, 11 while maintaining adhesion to the binder 70. Furthermore, sufficient adhesion to the current collector 20, 120 can be obtained while ensuring sufficient conductivity with the current collector 20, 120. At least a portion of the conductive network 80 is in contact with the core-shell particles 36, 136 and extends outward from the contact portion with the core-shell particles 36, 136. That is, the conductive network 80 has a conductive network cell contact portion that contacts the shell film 41 .

[0070] (Island-Shaped Portion 60) As shown in the enlarged view of FIG. 2( a), the island-shaped portion 60 is composed of coated active material particles 30 (130), a binder 70, and a conductive network 80. The island-shaped portion 60 is longer than the conductive paths between adjacent coated active material particles 30, 30 (130, 130), and the chain-like conductive network 80 forms the main skeleton of the island-shaped portion 60. The binder 70 supports the state in which the multiple coated active material particles 30 (130) are in contact with this conductive network 80. It is presumed that the potential equalization in the active material layer 21 (121) is carried out primarily by the long chain-like conductive network 80 made up of a conductive material, rather than by the conductive paths between the coated active material particles 30, 30 (130, 130). At least a portion of the conductive network 80 is exposed on the surface of the active material layer 21 (121). The reason why a structure is formed in which the binder 70 supports the state in which multiple coated active material particles 30 (130) are in contact with such a conductive network 80 is that, when produced using the manufacturing method described below, the slurry formed in the paste application process has coated active material particles 30 (130) with hydrophilic surfaces lined up in a hydrophobic medium containing a conductive material (conductive additive), binder 70, and solvent, and when the solvent is dried and removed, the coated active material particles are supported by the binder 70.

[0071] (Ocean-like portion 61) As shown in FIG. 2(a), the ocean-like portion 61 is composed of a permeable pore network 81. The permeable pore network 81 has a plurality of pores that are interconnected, allowing the electrolytic medium 6 to permeate. It is preferable that some of the pores of the permeable pore network 81 reach and contact the core-shell particles 36 (136). The permeable pore network 81 preferably has a pore-shell contact portion that contacts the shell membrane 41 via a buffer portion 42. The permeable pore network 81 has a non-liquid Li ion conductor having an SEI structure disposed at least in the contact portion (pore-shell contact portion). The Li ion conductor preferably contains one or more metal elements selected from Mn, Fe, Al, and Si. It is also preferable that the buffer portion 42 be formed from the pore-shell contact portion to the conductive network 80. The conductive network-cell contact portion, which is the contact portion between the conductive network 80 and the shell film 41, is preferably held between two adjacent pore-shell contact portions on the surface of the active material particle 40, 140.

[0072] From another perspective, the permeable pore network 81 is a cavity defined by the contours of the coated active material particles 30, the binder 70, and the conductive network 80, and is three-dimensionally continuous from the current collector 20 (120) side (inside) to the outside. On the surface of the active material particles 40 (140) or the shell film 41, the ratio of the total area of ​​the pores to the area of ​​the surface is preferably 0.1% or more and 30% or less, and more preferably 1% or more and 10% or less.

[0073] The permeable pore network 81 is in contact with the active material particles 40 (140) or the shell film 41, and a portion of the electrolytic medium 6 permeates therethrough at least during charging and discharging of the lithium-ion secondary battery 1, and a non-liquid Li ion conductor having an SEI structure is preferably formed in the contact portion of the permeable pore network 81. This non-liquid Li ion conductor having an SEI structure preferably contains one or more metal elements selected from the group consisting of Mn, Si, Fe, and Al, and more preferably contains Mn and Si.

[0074] (Separator 12) As shown in Fig. 1, the separator 12 is disposed between the positive electrode part 10 and the negative electrode part 11 and has a structure that is insulating and can contain the electrolytic medium 6. Examples of the separator 12 include woven fabrics, nonwoven fabrics, and microporous membranes made of nylon, cellulose, polysulfone, polyethylene, polypropylene, polybutene, polyacrylonitrile, polyimide, polyamide, polyethylene terephthalate, and composites of two or more of these. The separator 12 may contain various plasticizers, antioxidants, and flame retardants, and may be coated with metal oxides or the like.

[0075] (Positive Electrode Lead-Out Member 13 ) The positive electrode lead-out member 13 is a positive electrode terminal that is connected to one or more positive electrode parts 10 and can be connected to an external load, and is provided across the inside and outside of the exterior body 3 .

[0076] (Negative Electrode Lead-Out Member 14 ) The negative electrode lead-out member 14 is a negative electrode terminal that is connected to one or more negative electrode portions 11 and can be connected to an external load, and is provided across the inside and outside of the exterior body 3 .

[0077] <Electrolytic medium 6> The electrolytic medium 6 is an electrolytic solution, a polymer electrolyte, or a solid electrolyte, and is preferably a nonaqueous electrolytic solution in which a solute is dissolved in a nonaqueous solvent, or a polymer electrolyte in which a polymer is impregnated with a nonaqueous electrolytic solution in which a solute is dissolved in a nonaqueous solvent, and more preferably a nonaqueous electrolytic solution.

[0078] The nonaqueous solvent used in the electrolytic medium 6 preferably includes a cyclic aprotic solvent and / or a chain aprotic solvent. Examples of the cyclic aprotic solvent include cyclic carbonates, cyclic esters, cyclic sulfones, and cyclic ethers. From the viewpoint of forming a high-quality SEI structure, a cyclic carbonate-based compound containing an unsaturated bond or a halogen atom may be used. Examples of the chain aprotic solvent include solvents commonly used as solvents for nonaqueous electrolytes, such as chain carbonates, chain carboxylic acid esters, chain ethers, and acetonitrile. From the viewpoint of forming a high-quality SEI structure, a chain carbonate-based compound containing an unsaturated bond or a halogen atom may be used. More specifically, examples of aprotic solvents that can be used include dimethyl carbonate, methyl ethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, vinylene carbonate, γ-butyl lactone, 1,2-dimethoxyethane, sulfolane, dioxolane, and methyl propionate. These solvents may be used alone or in combination of two or more, but it is preferable to use a mixture of two or more solvents in view of the ease of dissolving the solute, which will be described later, and the high conductivity of Li ions.

[0079] When two or more aprotic solvents are mixed, a mixture of one or more chain carbonates exemplified by dimethyl carbonate, methyl ethyl carbonate, diethyl carbonate, dipropyl carbonate, and methyl propyl carbonate with one or more cyclic compounds exemplified by ethylene carbonate, propylene carbonate, butylene carbonate, and γ-butyrolactone is preferred, as this mixture has high stability at high temperatures and high lithium conductivity at low temperatures. A mixture of one or more chain carbonates exemplified by dimethyl carbonate, methyl ethyl carbonate, and diethyl carbonate with one or more cyclic carbonates exemplified by ethylene carbonate, propylene carbonate, and butylene carbonate is particularly preferred.

[0080] The solute used in the electrolytic medium 6 is not particularly limited, but may be, for example, LiClO 4 , LiBF 4 , LiPF 6 , LiAsF 6 , LiCF 3 SO 3 , LiBOB (Lithium Bis (Oxalato) Borate), LiN (SO 2 CF 3 ) 2 Lithium salts such as

[0081] The electrolytic medium 6 may further contain a silicon-containing compound as an additive. Examples of the silicon-containing compound include siloxane compounds, silazane compounds, and silylamide compounds containing one or more unsaturated groups, and among these, cyclic siloxanes having a vinyl group, such as 2,4,6,8-tetravinyl-2,4,6,8-tetramethylcyclotetrasiloxane (4VC4S), are preferred.

[0082] A siloxane-based compound containing one or more unsaturated groups contains a siloxane bond and at least one carbon double bond, and it is believed that the siloxane bond site can conduct Li ions and the carbon double bond site can contribute to the formation of an SEI structure through cross-linking.

[0083] The electrolytic medium 6 may be contained in advance in the positive electrode part 10 and the negative electrode part 11, or may be further contained in the separator 12. The electrolytic medium 6 may be added after the separator 12 is disposed between the positive electrode part 10 side and the negative electrode part 11 side and then wound or stacked.

[0084] When the electrolytic medium 6 is a polymer electrolyte, the electrolytic medium 6 may be made of PEG, PEO, PAn, PVDF, a fluorine-based polymer, or a polymer obtained by grafting a (meth)acrylic polymer onto a fluorine-based polymer.

[0085] When the electrolytic medium 6 is a solid electrolyte, the electrolytic medium 6 is preferably a ceramic electrolyte containing lithium element, for example, Li 10 GeP 2 S 12 (LGPS), Li 7 P3 S 11 , 70Li 2 S-30P 2 S 5 sulfide-based solid electrolytes such as (Li,La)TiO 3 and NASICON type solid electrolytes such as LATP.

[0086] The electrolytic medium 6 may further contain additives such as an electrode protectant, a gas generation inhibitor, an SEI forming agent, an SEI formation promoter, an SEI property improver, a stabilizer, a metal elution inhibitor, and a flame retardant.

[0087] Next, a method for manufacturing the lithium ion secondary battery 1 of this embodiment will be described.

[0088] The manufacturing method of the lithium ion secondary battery 1 of this embodiment is mainly composed of a coated active material forming process, a paste-coated current collector firing process, an electrode laminate forming process, a battery assembly creating process, an interface electrolyte injection process, a voltage application process, an electrolytic medium injection process, and an aging process.

[0089] <Coated Active Material Forming Step> The coated active material forming step is a step of forming the coated active material particles 30, 130. The coated active material forming step is mainly composed of an active material particle preparing step, a shell film forming step, and a paste applying step.

[0090] (Active Material Particle Preparation Step) The active material particle preparation step is a step of preparing the active material particles 40 and 140 .

[0091] (Shell Film Forming Step) The shell film forming step is a step of forming shell films 41, 41 which are phosphate ion-containing lithium compound films on the surfaces of the active material particles 40, 140.

[0092] Specifically, the shell film formation process for forming the shell film 41 on the positive electrode active material particles 40 involves first pulverizing a phosphate ion-containing lithium compound using a pulverizing device such as a ball mill to form particles of the phosphate ion-containing lithium compound (pulverizing process).

[0093] Here, the phosphate ion-containing lithium compound before the pulverization step is preferably a Li ion conductive oxide containing phosphorus, and more preferably a phosphate-based compound having an olivine-type crystal structure. The phosphate ion-containing lithium compound particles after the pulverization step preferably have a partially destroyed crystal structure and are wholly or partially amorphous. When the phosphate ion-containing lithium compound particles after the pulverization step are entirely amorphous, when the phosphate ion-containing lithium compound particles are measured by an X-ray diffraction (XRD) method, the inherent crystalline peaks of the phosphate ion-containing lithium compound that appeared before the pulverization step are not observed as a halo pattern.

[0094] Furthermore, the particles of the phosphate ion-containing lithium compound after the pulverization step have a BET specific surface area of ​​20 m 2 / g or more 80m 2 / g or less. After the pulverization process, the particles of the phosphate ion-containing lithium compound preferably have a BET specific surface area equivalent diameter (dBET) of 30 nm or more, more preferably 50 nm or more. After the pulverization process, the particles of the phosphate ion-containing lithium compound preferably have a BET specific surface area equivalent diameter (dBET) of 500 nm or less, more preferably 450 nm or less. Within these ranges, the surfaces of the active material particles 40, 140 can be uniformly coated, and a dense shell film 41 can be formed. The BET specific surface area equivalent diameter (dBET) is a particle size calculated by determining the nitrogen adsorption BET specific surface area using the nitrogen adsorption single-point method in accordance with the method specified in JIS Z8830 (2013), and then applying the formula dBET = 6 / (density × BET specific surface area).

[0095] Subsequently, the mixture is pulverized in a pulverization step, and the resulting fine particles of the phosphate ion-containing lithium compound are dispersed in a dispersion solvent to form a fine particle fluid (fine particle fluid formation step).

[0096] The dispersion solvent used in this case is preferably one or more alcohol solutions, and more preferably ethanol from the viewpoints of volatility and safety. The microparticle fluid formed in this case is a transparent sol in a sol state and has fluidity.

[0097] Next, a mechanical coating method is used to mechanically contact the active material particles 40 with the particles of the phosphate ion-containing lithium compound in the microparticle fluid, while applying at least one type of energy selected from shear force, compression force, collision force, and centrifugal force to the active material particles 40 and / or the particles of the phosphate ion-containing lithium compound that constitute the shell film 41, thereby forming the shell film 41 on the surface of each active material particle 40. In this embodiment, the microparticle fluid is milled into the active material particles 40 using a milling device such as a milling mill, to form a milled product (milled product formation step).

[0098] The amount of phosphate ion-containing lithium compound particles added to the milling device is preferably 0.5 wt % or more. The amount of phosphate ion-containing lithium compound particles added to the milling device is preferably 2.5 wt % or less, more preferably 1.6 wt % or less, and particularly preferably 1 wt % or less. The treatment temperature in the milling device is preferably 5°C or higher and 100°C or lower, more preferably 8°C or higher and 80°C or lower, and even more preferably 10°C or higher and 50°C or lower. The treatment time in the milling device is preferably 5 minutes or higher and 90 minutes or lower, and more preferably 10 minutes or higher and 60 minutes or lower. The atmosphere in the milling device is preferably an inert gas atmosphere or an air atmosphere.

[0099] Next, the ground product is subjected to a heat treatment to remove the dispersion solvent from the ground product, forming a shell film 41 and forming core-shell particles 36 (removal step).

[0100] The heat treatment temperature is preferably 300°C or higher, more preferably 350°C or higher. If the heat treatment temperature is lower than 300°C, the adhesion between the active material particles 40 and the shell film 41 will be insufficient, which may cause the shell film 41 to peel off during charging and discharging of the battery, resulting in a decrease in the long-term reliability of the battery. On the other hand, if the heat treatment temperature is too high, the crystalline structure of the shell film 41 may change, reducing the Li ion conductivity and preventing normal charging and discharging of the battery. Therefore, the heat treatment temperature is preferably 850°C or lower, more preferably 500°C or lower from the viewpoint of suppressing crystallization of the amorphous portion of the shell film 41. The heat treatment time is preferably 30 minutes or longer, more preferably 45 minutes or longer. The heat treatment time is preferably 180 minutes or shorter, more preferably 150 minutes or shorter.

[0101] The above is a description of the shell film formation process in which shell film 41, which is a phosphate ion-containing lithium compound film, is formed on the surface of positive electrode active material particles 40. The shell film formation process in which shell film 41, which is a phosphate ion-containing lithium compound film, is formed on the surface of negative electrode active material particles 140 is similar except that negative electrode active material particles 140 are used instead of positive electrode active material particles 40, and therefore a description thereof will be omitted. In other words, the shell film formation process in which shell film 41 is formed on positive electrode active material particles 40 and the shell film formation process in which shell film 41 is formed on negative electrode active material particles 140 are basically similar, with the difference being whether the core is positive electrode active material particles 40 or negative electrode active material particles 140.

[0102] (Paste application process) The paste application process is a process in which the active material particles 40, 140 (core-shell particles 36, 136) on which the shell film 41, 41 is formed are mixed with a conductive material, a binder 70, and optionally a silicon-containing compound, dispersed in a solvent to form a paste-like slurry, and the slurry is applied to the current collector 20, 120 to form a paste-coated current collector.

[0103] The solvent used in this step is not particularly limited as long as it can dissolve or disperse the core-shell particles 36, 136, the conductive material that constitutes the conductive network 80, and the binder 70, but examples of solvents that can be used include N-methyl-2-pyrrolidone (NMP), dimethylformamide, dimethylacetamide, methyl ethyl ketone, methyl acetate, ethyl acetate, and tetrahydrofuran. A dispersant and a thickener may also be added to these solvents.

[0104] <Pasted Current Collector Firing Step> The pasted current collector firing step is a step of firing the pasted current collector for a predetermined firing time at a predetermined firing temperature to form a positive electrode part in progress containing positive electrode active material particles 40 and a negative electrode part in progress containing negative electrode active material particles 140. The firing temperature is not particularly limited as long as it is a temperature at which the pasted current collector is fired and the slurry solidifies, but is preferably, for example, 80°C or higher and 200°C or lower.

[0105] At this time, the solvent in the paste-coated current collector is evaporated and removed, forming pores, and a permeable pore network 81 is formed in the in-process positive electrode portion and in-process negative electrode portion.

[0106] <Electrode Stack Forming Step> The electrode stack forming step is a step of forming an in-progress electrode stack by sandwiching a separator 12 between an in-progress positive electrode part and an in-progress negative electrode part.

[0107] <Battery Assembly Fabrication Process> The battery assembly fabrication process is a process in which a work-in-progress electrode stack is placed inside the exterior case 3 to fabricate a work-in-progress battery assembly.

[0108] <Interface Electrolyte Injection Step> The interface electrolyte injection step is a step of, for example, using a vacuum packaging machine to reduce the internal pressure to 0.1 atmospheres or less, sealing the exterior body 3 containing the in-progress electrode stack therein except for the injection port, and then injecting the interface electrolyte into the exterior body 3 of the in-progress battery assembly. The interface electrolyte has Li ion conductivity and contains a silicon-containing compound that is the material for the buffer section 42. The interface electrolyte contains lithium and silicon. For example, the interface electrolyte may be one that contains the electrolytic medium 6 described above and, in addition, a vinyl group-containing cyclic siloxane such as 2,4,6,8-tetravinyl-2,4,6,8-tetramethylcyclotetrasiloxane (4VC4S) as an additive.

[0109] <Voltage Application Step> The voltage application step is a step of applying a voltage between the positive electrode take-out member 13 and the negative electrode take-out member 14 of the in-progress electrode laminate. By the voltage application step, the silicon-containing compound in the interface electrolyte is layered on the shell film 41 of the core-shell particles 36, 136 of the in-progress electrode laminate, forming a buffer section 42 including a modified region in which the SEI structure is modified by siloxane bonding, and forming an electrode laminate 5 including a positive electrode section 10 and a negative electrode section 11. The voltage applied between the positive electrode take-out member 13 and the negative electrode take-out member 14 in this step is a voltage at which the silicon-containing compound in the interface electrolyte precipitates on the surface of the shell film 41, and is 4.5 V or more and 5 V or less (vs. Li + / Li).

[0110] <Electrolytic Medium Injection Step> The electrolytic medium injection step is a step of discharging the interface electrolyte from the exterior body 3 as needed, and injecting the electrolytic medium 6 into the exterior body 3 of the battery assembly 2 .

[0111] <Aging Process> The aging process is a process for checking for initial deterioration of the battery assembly 2, and is composed of an initial charging process and a curing process. The initial charging process is a process for charging by applying a voltage between the positive electrode take-out member 13 and the negative electrode take-out member 14 of the electrode stack 5. The curing process is a process for curing the exterior body 3 to seal the electrode stack 5 and the electrolytic medium 6.

[0112] In the lithium-ion secondary battery 1 of this embodiment, the coating 35 coating the active material particles 40, 140 contains a phosphate-containing lithium compound, thereby suppressing gas generation due to decomposition of the electrolytic medium 6. In the lithium-ion secondary battery 1 of this embodiment, the shell film 41 preferably contains one or more metals selected from the group consisting of Fe, Mn, Si, and Al, and more preferably the shell film 41 uniformly coats the active material particles 40, 140. This reduces the area of ​​contact between the active material particles 40, 140 and the electrolytic medium 6, thereby suppressing gas generation due to decomposition of the electrolytic medium 6. In the lithium-ion secondary battery 1 of this embodiment, the positive electrode active material particles 40 are preferably composed of a LiMn-based oxide and are coated with a shell film 41 made of a phosphate-based compound that can also be used as a positive electrode active material. This facilitates smooth insertion and desorption reactions of Li ions. In the lithium-ion secondary battery 1 of this embodiment, the positive electrode active material particles 40 are preferably composed of a nickel-containing LiMn-based oxide, for example, a LiMn-based oxide having a spinel-type crystal structure. This allows for the construction of a high-capacity secondary battery capable of generating high voltages. In the lithium-ion secondary battery 1 of this embodiment, the positive electrode active material particles 40 are preferably composed of a layered rock-salt oxide, and more preferably, a LiMn-based oxide having a Li-excess layered rock-salt structure. This allows for the construction of an even higher-capacity secondary battery. In the lithium-ion secondary battery 1 of this embodiment, the negative electrode active material particles 140 are preferably composed of a Li-titanium-based oxide. This allows for the construction of a secondary battery with excellent safety and reliability. In the lithium-ion secondary battery 1 of this embodiment, the negative electrode active material particles 140 are preferably coated with a shell film 41 of a phosphate-based compound that can also be used as a positive electrode active material. This allows for smooth Li-ion insertion and desorption reactions, allowing for the construction of a secondary battery with excellent characteristics.

[0113] In the lithium-ion secondary battery 1 of this embodiment, the vicinity of the interface between the shell film 41 and the active material particles 40, 140 is amorphous, and therefore the amorphous portion of the shell film 41 functions as a buffer even when the volume of the active material particles 40, 140 changes as charging and discharging proceeds. Therefore, cracking and peeling of the shell film 41 and, in turn, the coating 35 are less likely to occur. In the lithium-ion secondary battery 1 of this embodiment, a fine particle fluid in which fine particles, the raw material of the shell film 41, are dispersed in a dispersion solvent is milled into the active material particles 40, 140, and heat treatment is performed at a temperature of 100°C or higher and 500°C or lower. This makes it possible to form a high-quality, thin shell film 41 on the surface of the active material particles 40 while maintaining the amorphous state.

[0114] According to the lithium ion secondary battery 1 of this embodiment, the shell films 41, 41, which are part of the coating 35 that covers the active material particles 40, 140, contain a phosphate ion-containing lithium compound, so that the generation of gas due to decomposition of the electrolytic medium 6 can be further suppressed.

[0115] In the lithium ion secondary battery 1 of this embodiment, the shell film 41 contains a phosphate ion-containing lithium compound containing one or more metals selected from the group consisting of Fe, Mn, Si, and Al, which can suppress the generation of gas due to decomposition of the electrolytic medium 6. In the lithium ion secondary battery 1 of this embodiment, the active material layer 21, 121 has the conductive network 80 and the permeable pore network 81, which facilitates the exchange of charges and lithium ions between the electrolytic medium 6 and the active material particles 40, 140, making it easier for an electrode reaction to occur.

[0116] According to the lithium ion secondary battery 1 of this embodiment, the permeable pore network 81 has a lithium ion conductor provided from the contact portion with the active material particles 40, 140 or the shell membrane 41, 41 toward the pores, thereby making the exchange of charges and lithium ions between the electrolytic medium 6 and the active material particles 40, 140 smoother and making it easier for electrode reactions to occur.

[0117] According to the lithium ion secondary battery 1 of this embodiment, the buffering portion 42 has a silicon-containing compound film containing elemental silicon, so that the binding property of the buffering portion 42 is improved and cracks and the like are less likely to occur.

[0118] According to the lithium ion secondary battery 1 of this embodiment, the shell film 41 contains lithium elements, and the lithium in the shell film 41 can be used to replenish lithium consumed for some reason, so performance is less likely to deteriorate.

[0119] According to the lithium ion secondary battery 1 of this embodiment, the shell film 41 can suppress the elution of manganese element from the positive electrode active material particles 40 into the electrolytic medium 6, so that the performance is less likely to deteriorate.

[0120] In the above-described embodiment, the buffer section 42 is formed by injecting an interface electrolyte in the interface electrolyte injection step and applying a voltage between the positive electrode take-out member 13 and the negative electrode take-out member 14 in the voltage application step, but the present invention is not limited to this. For example, a silicon-containing compound containing silicon element may be added to the slurry in the paste application step, and the buffer section 42 may be formed in the paste-applied current collector firing step. Alternatively, the buffer section 42 may be formed by applying a paste containing a silicon-containing compound to the in-process positive electrode section and the in-process negative electrode section after the paste-applied current collector firing step, and then solidifying the paste by heating, ultraviolet light, or the like. The buffer section 42 may be formed by applying a paste containing a silicon-containing compound to the in-process electrode stack after the electrode stack formation step, and then solidifying the paste by heating, ultraviolet light, or the like.

[0121] In the above-described embodiment, the buffer section 42 is formed, but the present invention is not limited to this, and it is also possible not to form the buffer section 42. In this case, the battery assembly fabrication step, the interface electrolyte injection step, and the voltage application step are omitted, and the electrolytic medium injection step is performed after the battery assembly fabrication step.

[0122] In the above-described embodiments, each component can be freely substituted or added between the respective embodiments as long as it falls within the technical scope of the present invention.

[0123] The present invention will be specifically described below with reference to examples. Note that the present invention is not limited to the following examples and can be practiced with appropriate modifications within the scope of the present invention.

[0124] (Experimental Example 1) (i) Preparation of Positive Electrode First, a predetermined amount of ethanol solvent was mixed with lithium manganese phosphate (hereinafter also referred to as LMP) powder having an olivine crystal structure, and the mixture was treated in a planetary ball mill using zirconia balls with a diameter of 0.5 mm for 3 hours. After the treatment, the zirconia balls were removed from the mixture using a sieve, and the mixture was dried at 120°C to remove the ethanol, yielding an LMP fine powder. Next, the LMP fine powder and ethanol were mixed to obtain a slurry of LMP fine powder dispersed in ethanol with a solid content of 16.4 wt%.

[0125] The positive electrode active material was a spinel-type lithium nickel manganese oxide (LiNi) with a median diameter of 5 μm. 0.5 Mn 1.5 O 4 (hereinafter, also referred to as LNMO) was used. 30 g of LNMO was placed in a grinding mill (manufactured by Hosokawa Micron Corporation, product name: Nobilta), and while rotating at 2600 rpm with a clearance of 0.6 mm and a rotor load power of 1.5 kW, an ethanol-dispersed slurry of LMP fine powder was added in two portions so that the amount of LMP fine powder added was 0.6 wt %. Thereafter, the rotor rotation speed was maintained in the range of 2600 rpm to 3000 rpm, and the mixture was treated at room temperature in an air atmosphere for 10 minutes to obtain LNMO whose surface was coated with LMP. The obtained surface-coated LNMO was heat-treated at 350°C for 1 hour to obtain a positive electrode composite active material.

[0126] A mixture containing the obtained positive electrode composite active material, acetylene black as a conductive material, and polyvinylidene fluoride (PVdF) as a binder in solid concentrations of 90 parts by weight, 6 parts by weight, and 4 parts by weight, respectively, was dispersed in N-methyl-2-pyrrolidone (NMP) to prepare a slurry. The binder was prepared as an N-methyl-2-pyrrolidone (NMP) solution with a solid concentration of 5% by weight, and NMP was further added to adjust the viscosity to facilitate coating, as described below.

[0127] The slurry was applied to a 20 μm thick aluminum foil and then dried in an oven at 120° C. This operation was performed on both sides of the aluminum foil, and then the foil was further dried in a vacuum at 170° C. to prepare a positive electrode.

[0128] (ii) Preparation of negative electrode As a negative electrode active material, spinel-type lithium titanate (Li 4 Ti 5 O 12 (hereinafter, also referred to as LTO) was used. A mixture containing 100 parts by weight of the LTO, acetylene black as a conductive additive, and 5 parts by weight of polyvinylidene fluoride (PVdF) as a binder, respectively, in terms of solid content, was dispersed in N-methyl-2-pyrrolidone (NMP) to prepare a slurry. The binder used was an NMP solution with a solid content of 5 wt %, and NMP was further added to adjust the viscosity to facilitate coating, as described below.

[0129] The slurry was applied to a 20 μm thick aluminum foil and then dried in an oven at 120° C. This operation was performed on both sides of the aluminum foil, and then the foil was further dried in a vacuum at 170° C. to prepare a negative electrode.

[0130] (iii) Fabrication of Lithium-Ion Secondary Battery A battery was fabricated using the positive and negative electrodes fabricated in (i) and (ii) above and a 20 μm polypropylene separator according to the following procedure. First, the positive and negative electrodes were dried under reduced pressure at 80° C. for 12 hours. Next, 15 positive electrodes and 16 negative electrodes were stacked in the order of negative electrode / separator / positive electrode. Both outermost layers were separators. Next, aluminum tabs were vibration-welded to both ends of the positive and negative electrodes.

[0131] Two aluminum laminate films were prepared as exterior materials, and a recess for the battery portion and a recess for the gas collection portion were formed by pressing. The electrode stack was then placed inside. The outer periphery, leaving a space for the non-aqueous electrolyte injection, was heat-sealed at 180°C for 7 seconds, and the unsealed portion was filled with LiPF in a solvent made by mixing ethylene carbonate, propylene carbonate, and ethyl methyl carbonate in a volume ratio of ethylene carbonate / propylene carbonate / ethyl methyl carbonate = 15 / 15 / 70. 6The non-aqueous electrolyte was added and the unsealed areas were heat-sealed at 180°C for 7 seconds while the pressure was reduced. The resulting battery was charged at a constant current equivalent to 0.2 C until the battery voltage reached a cut-off voltage of 3.4 V, and then the charging was stopped. The battery was then left to stand for 24 hours in a 60°C environment, after which it was discharged at a constant current equivalent to 0.2 C. The discharge was stopped when the battery voltage reached 2.5 V. After the discharge was stopped, the gas accumulated in the gas collection section was removed and the battery was resealed. A lithium-ion secondary battery for evaluation was fabricated using the above procedures.

[0132] (Experimental Example 2) (i) In the preparation of the positive electrode, the same procedure as in Experimental Example 1 was carried out except that the coating amount of the LMP fine powder was adjusted to 0.9 wt %. This was designated as Experimental Example 2.

[0133] (Experimental Example 3) (i) In the preparation of the positive electrode, the same procedure as in Experimental Example 1 was carried out except that the coating amount of the LMP fine powder was adjusted to 1.5 wt %. This was designated as Experimental Example 3.

[0134] (Experimental Example 4) (i) In the production of the positive electrode, LiFePO having an olivine-type crystal structure was used instead of LMP fine powder. 4 (hereinafter also referred to as LFP) was used, and the coating amount of the LFP fine powder was adjusted to 1.2 wt %, and the same procedure as in Experimental Example 1 was carried out. This was designated Experimental Example 4.

[0135] (Experimental Example 5) (i) Experimental Example 5 was prepared in the same manner as in Experimental Example 4, except that the coating amount of the LFP fine powder was adjusted to 2.4 wt % in the preparation of the positive electrode.

[0136] (Experimental Example 6) (i) In the preparation of the positive electrode, Li was used instead of LMP. 1.3 Al 0.3 Ti 1.7 (P.O. 4 ) 3 (hereinafter also referred to as LATP) was used, and the coating amount of the LATP fine powder was adjusted to 1.2 wt %, and the same procedure as in Example 4 was carried out to prepare Example 6. The LATP fine powder was prepared by the following method. 2 CO 3 , AlPO4 , TiO 2 , N.H. 4 H 2 P.O. 4 The mixture was mixed with a predetermined amount of ethanol as a solvent and treated in a planetary ball mill at 150 G for 1 hour using zirconia balls with a diameter of 3 mm. The zirconia balls were removed from the treated mixture using a sieve, and the mixture was dried at 120 °C to remove the ethanol. The mixture was then treated at 800 °C for 2 hours to obtain a fine powder of LATP.

[0137] (Experimental Example 7) (i) In the preparation of the positive electrode, the same procedure as in Experimental Example 4 was carried out except that the coating amount of the LATP fine powder was adjusted to 2.4 wt %. This was designated as Experimental Example 7.

[0138] (Experimental Example 8) (i) In the preparation of the positive electrode, the same procedure as in Experimental Example 1 was carried out except that the surface-coated LNMO was heat-treated at 450°C for 1 hour to obtain a positive electrode composite active material. This was designated as Experimental Example 8.

[0139] (Experimental Example 9) (i) In the preparation of the positive electrode, the same procedure as in Experimental Example 1 was carried out except that the surface-coated LNMO was heat-treated at 800° C. for 1 hour to obtain a positive electrode composite active material. This was designated Experimental Example 9.

[0140] (Experimental Example 10) (i) In the preparation of the positive electrode, the same procedure as in Experimental Example 2 was conducted except that the surface-coated LNMO was heat-treated at 450° C. for 1 hour to obtain a positive electrode composite active material. This was designated Experimental Example 10.

[0141] (Experimental Example 11) (i) In the preparation of the positive electrode, the same procedure as in Experimental Example 2 was carried out except that the surface-coated LNMO was heat-treated at 800° C. for 1 hour to obtain a positive electrode composite active material. This was designated Experimental Example 11.

[0142] (Experimental Example 12) (i) In the preparation of the positive electrode, the same procedure as in Experimental Example 1 was carried out except that the surface-coated LNMO was heat-treated at 350° C. for 2 hours to obtain a positive electrode composite active material. This was designated Experimental Example 12.

[0143] (Experimental Example 13) (i) In the preparation of the positive electrode, the same procedure as in Experimental Example 2 was conducted except that the surface-coated LNMO was heat-treated at 350°C for 2 hours to obtain a positive electrode composite active material. This was designated Experimental Example 13.

[0144] (Experimental Example 14) (i) In the preparation of the positive electrode, the coating amount of LATP fine powder was adjusted to 1.2 wt %, and the surface-coated LNMO was heat-treated at 400 °C for 1 hour to obtain a positive electrode composite active material. (ii) In the preparation of the negative electrode, (i) following the preparation of the positive electrode, LTO was used as the negative electrode active material. 30 g of LTO was placed in a grinding mill. While rotating at 2600 rpm with a clearance of 0.6 mm and a rotor load power of 1.5 kW, an ethanol-dispersed slurry of LMP fine powder was added in two portions so that the LMP fine powder loading amount was 2.4 wt %. The rotor rotation speed was then maintained in the range of 2600 rpm to 3000 rpm, and the mixture was treated at room temperature in an air atmosphere for 10 minutes to obtain LTO with a surface coated with LMP. The obtained surface-coated LTO was heat-treated at 350° C. for 1 hour to obtain a negative electrode composite active material.

[0145] A mixture containing the obtained negative electrode composite active material, acetylene black as a conductive material, and polyvinylidene fluoride (PVdF) as a binder in solid concentrations of 90 parts by weight, 6 parts by weight, and 4 parts by weight, respectively, was dispersed in N-methyl-2-pyrrolidone (NMP) to prepare a slurry. The binder was prepared as an N-methyl-2-pyrrolidone (NMP) solution with a solid concentration of 5% by weight, and NMP was further added to adjust the viscosity to facilitate coating, as described below.

[0146] The slurry was applied to a 20 μm thick aluminum foil and then dried in an oven at 120° C. This operation was repeated on both sides of the aluminum foil, and then the foil was further dried in a vacuum at 170° C. to prepare a negative electrode. Other than the above, the procedure was the same as in Experimental Example 6, and this was designated Experimental Example 14.

[0147] (Experimental Example 15) (ii) In the preparation of the negative electrode, the same procedure as in Experimental Example 14 was conducted except that the surface-coated LTO was heat-treated at 600° C. for 1 hour to obtain a negative electrode composite active material. This was designated Experimental Example 15.

[0148] (Experimental Example 16) (ii) In preparing the negative electrode, the procedure was the same as in Experimental Example 14, except that LFP was used instead of LMP and the coating amount of LFP fine powder was adjusted to 2.4 wt %, and this was designated Experimental Example 16.

[0149] (Experimental Example 17) (ii) In the preparation of the negative electrode, the same procedure as in Experimental Example 16 was carried out except that the surface-coated LTO was heat-treated at 600°C for 1 hour to obtain a negative electrode composite active material. This was designated Experimental Example 17.

[0150] (Experimental Example 18) (i) In the preparation of a positive electrode, the same procedure as in Experimental Example 1 was carried out except that LNMO was used as it was without forming a coating, and this was designated as Experimental Example 18. That is, in Experimental Example 18, LNMO was used for the positive electrode and LTO was used for the negative electrode.

[0151] (Measurement of Gas Generation Amount) The amount of gas generated from the lithium ion secondary battery before and after the cycle characteristic evaluation in each of Experimental Examples 1 to 18 was evaluated using the Archimedes method, that is, the buoyancy of the lithium ion secondary battery. The evaluation was performed as follows.

[0152] First, the weight of the lithium-ion secondary battery was measured using an electronic balance. Next, the weight in water was measured using a hydrometer (manufactured by Alpha Mirage, product number: MDS-3000), and the buoyancy was calculated by taking the difference between these weights. The volume of the lithium-ion secondary battery was calculated by dividing this buoyancy by the density of water (1.0 g / cm). The volume after aging and the volume after the cycle characteristic evaluation described below were compared to calculate the amount of gas generated.

[0153] (Evaluation of Cycle Characteristics of Lithium-Ion Secondary Battery) The lithium-ion secondary batteries prepared in each of Experimental Examples 1 to 18 were connected to a charge / discharge device (HJ1005SD8, manufactured by Hokuto Denko Corporation) and cycled. Constant-current charging was performed at a current value equivalent to 1.0 C in a 60°C environment until the battery voltage reached a cut-off voltage of 3.4 V, and charging was then stopped. Subsequently, constant-current discharging was performed at a current value equivalent to 1.0 C, and discharging was stopped when the battery voltage reached 2.5 V. This constituted one cycle, and charging and discharging were repeated. The stability of the cycle characteristics was evaluated as the capacity retention rate (%), where the discharge capacity at the 500th cycle was taken as 100.

[0154] (Rate characteristic evaluation) The lithium ion secondary batteries produced in each of Experimental Examples 1 to 18 were charged and discharged at 25° C. at 0.2 C, followed by charging and discharging at 2.0 C, to evaluate the rate characteristics. The end-of-charge voltage and end-of-discharge voltage were set to 2.5 V and 3.4 V, respectively. The ratio of the discharge capacity at 2.0 C to the discharge capacity at 0.2 C was defined as the discharge rate characteristic.

[0155] First, the evaluation results of each of Experimental Examples 1 to 7 are shown in Table 1.

[0156]

[0157] In Experimental Examples 1 to 7 in which a coating was formed, the amount of gas generated after 100 cycles was suppressed to 10 cc / Ah or less, as shown in Table 1. This suggests that the formation of a coating has the effect of suppressing gas generation (hereinafter also referred to as gas generation suppression effect).

[0158] As shown in Table 1, Experimental Examples 1 to 3, in which LMP was used as the coating, showed improved rate characteristics compared to Experimental Examples 4 and 5, in which LFP was used as the coating, and Experimental Examples 6 and 7, in which LATP was used as the coating. In Experimental Examples 4 and 5, in which LFP was used as the coating, and Experimental Examples 6 and 7, in which LATP was used, as the amount added increased, the initial capacity decreased, the 2C value also decreased, and the amount of gas generated decreased. On the other hand, in Experimental Examples 1 to 3, in which LMP was used as the coating, as the amount of coating added increased, the initial capacity increased, the 2C value remained almost constant, and the amount of gas generated increased. This suggests that when LMP is used as the coating, the capacity is maintained even if the amount of coating added is small, and the effect of suppressing gas generation is high.

[0159] Next, the evaluation results of Experimental Examples 1, 2, and 8 to 11 are shown in Table 2.

[0160]

[0161] As shown in Table 2, in each of Experimental Examples 1, 2, and 8 to 11, the gas generation rate after 100 cycles was suppressed to 10 cc / Ah or less. Although there was concern about the occurrence of cracks as the treatment temperature increased, no clear increase in the gas generation rate was observed even when heat treatment was performed at 800°C. Furthermore, when comparing Experimental Examples 1, 8, and 9, which contained 0.6 wt% additive, the initial capacity and 2C values ​​increased as the treatment temperature increased. Similarly, when comparing Experimental Examples 2, 10, and 11, which contained 0.9 wt%, the initial capacity and 2C values ​​increased as the treatment temperature increased. These findings suggest that increasing the treatment temperature increases the initial capacity and 2C values ​​while suppressing gas generation.

[0162] Next, the evaluation results of Experimental Examples 1, 2, 12, and 13 are shown in Table 3.

[0163]

[0164] In each of Experimental Examples 1, 2, 12, and 13, the amount of gas generated after 100 cycles was kept below 10 cc / Ah, as shown in Table 3. In Experimental Examples 1 and 12, in which the amount of coating added was 0.6 wt%, the amount of gas generated after 100 cycles and the amount of gas generated after 300 cycles hardly changed with increasing treatment time. In Experimental Examples 1 and 12, in which the amount of coating added was 0.6 wt%, the amount of gas generated after 300 cycles was lower than in Experimental Examples 2 and 13, in which the amount of coating added was 0.9 wt%. Furthermore, in Experimental Examples 1, 2, 12, and 13, the initial capacity and 2C value increased with increasing treatment time.

[0165] These findings suggest that extending the treatment time improves the uniformity of the coating and the gas suppression effect. Furthermore, extending the treatment time also restores the initial capacity, suggesting that adding a small amount to form a thin coating increases the coating effect.

[0166] Next, the evaluation results of each of Experimental Examples 14 to 18 are shown in Table 4.

[0167]

[0168] In Experimental Examples 14 to 17, in which a coating was formed, the rate characteristics were almost the same as in Experimental Example 18, in which a coating was not formed. However, the amount of gas generated after 500 cycles was reduced to 35 cc / Ah or less, and the capacity retention rate was also improved. This suggests that forming a coating on the negative electrode can also achieve a gas generation suppression effect. Furthermore, when Experimental Examples 14 and 15 are compared, the rate characteristics improved as the treatment temperature increased. Similarly, when Experimental Examples 16 and 17 are compared, the rate characteristics improved as the treatment temperature increased. This suggests that the rate characteristics can be improved by increasing the treatment temperature. In Experimental Examples 14 and 15, in which LMP was coated, the amount of gas generated was reduced and the rate characteristics were improved compared to Experimental Examples 16 and 17, in which LFP was coated.

[0169] From the above, it was found that the amount of gas generation can be suppressed by coating the surface of the active material particles with a film containing a phosphate ion-containing lithium compound. In particular, it was found that the amount of gas generation can be suppressed and the rate characteristics can be improved by coating the surface of the active material particles with LMP.

[0170] REFERENCE SIGNS LIST 1 Lithium ion secondary battery 3 Exterior body 5 Electrode laminate 6 Electrolytic medium (electrolyte) 10 Positive electrode portion 11 Negative electrode portion 21 Positive electrode active material layer 30, 130 Coated active material particle 35 Coating 36, 136 Core-shell particle 40 Positive electrode active material particle 41 Shell film 42 Buffer portion 60 Island portion 61 Sea portion 70 Binder 80 Conductive network 81 Permeable pore network 121 Negative electrode active material layer 140 Negative electrode active material particle

Claims

1. Coated active material particles in which active material particles are coated with a coating, the coating containing a phosphate ion-containing lithium compound that contains lithium ions, a metal species, and phosphate ions.

2. The coated active material particles according to claim 1, wherein the phosphate ion-containing lithium compound contains manganese element.

3. The coated active material particles according to claim 1, wherein the phosphate ion-containing lithium compound contains elemental silicon.

4. The coated active material particles according to claim 1, wherein both surfaces of the coating are different in at least one of the concentration of the phosphate ions, the concentration of the metal species, and the composition.

5. The coated active material particle according to claim 1, comprising a core-shell particle having a core-shell structure in which the active material particle constitutes a core and a continuous shell film constitutes the shell, the shell film constitutes the outer surface of the core-shell particle, the coating has the shell film and a buffer section in that order from the active material particle side, the buffer section is formed and distributed on the outer surface of the shell film, and the coating has at least one of the concentration of the phosphate ions, the concentration of the metal species, and a composition that differs on both sides of the shell film.

6. The coated active material particle according to claim 5, wherein the coating has at least one different concentration of the phosphate ions, the concentration of the metal species, and the composition on both sides of the buffer portion.

7. The coated active material particle according to claim 5, wherein the average occupancy rate of the buffer portion relative to the outer surface of the shell film per active material particle is 0.1% or more and 30% or less.

8. An active material layer comprising the coated active material particles according to any one of claims 1 to 7, wherein the coating has a shell film in contact with the active material particles, the shell film contains the phosphate ion-containing lithium compound, the phosphate ion-containing lithium compound contains one or more metals selected from the group consisting of Fe, Mn, Si and Al, the active material layer having a cross-sectional island structure, comprising an island portion and a sea portion, the island portion including a permeable pore network, and the sea portion including the active material particles, a binder and a conductive network.

9. An active material layer as described in claim 8, wherein at least a portion of the conductive network is in contact with the active material particles or the shell film, the permeable pore network has pores and is at least partially in contact with the active material particles or the shell film, and the permeable pore network has a lithium ion conductor provided from the contact portion with the active material particles or the shell film toward the pores.

10. The active material layer according to claim 8, wherein the active material particles are negative electrode active material particles for a lithium ion secondary battery and contain lithium titanate.

11. The active material layer according to claim 8, wherein the active material particles are positive electrode active material particles for a lithium ion secondary battery and contain lithium nickel manganese oxide.

12. An active material layer containing active material particles for a lithium ion secondary battery, the active material layer having a cross-sectional shape of a sea-island structure, the active material layer having island-like portions and a sea-like portion, the island-like portions including a permeable pore network, and the sea-like portion including the active material particles, a binder, and a conductive network.

13. An active material layer as described in claim 12, wherein the active material particles are coated active material particles coated with a coating, the coating is a multilayer film including at least two layers, a shell film and a buffer section from the active material particle side, the conductive network is made of a conductive material and has a conductive network cell contact section in contact with the shell film, and the permeable pore network has a pore shell contact section in contact with the shell film via the buffer section.

14. An active material layer as described in claim 13, wherein the buffer portion is formed from the pore-shell contact portion to the conductive network, and the conductive network-cell contact portion is held between two adjacent pore-shell contact portions on the surface of the active material particle.

15. A lithium ion secondary battery in which an electrode laminate having a positive electrode and a negative electrode facing each other with an electrolyte sandwiched therebetween is enclosed within an exterior body, wherein the positive electrode or the negative electrode contains the coated active material particles according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Positive electrode active material for lithium ion secondary battery

    JP2018116856A

  • Positive electrode active material composite for lithium ion secondary battery and method for producing the same

    JP2021048037A

  • Positive electrode active material powder

    JP2022022256A

  • Positive electrode active material for lithium ion secondary battery, and manufacturing method of lithium ion secondary battery

    JP2022130217A

  • Positive electrode and non-aqueous electrolyte secondary battery including the same

    JP2022141208A

Cited By

  • Lithium ion secondary battery

    JP2026093828A

  • Secondary battery

    WO2026094321A1