Electrode catalyst layer and membrane electrode assembly

The integration of ionomer-adsorbing carbon fibers and coated fibers with specific functional groups in the electrode catalyst layer addresses crack issues, enhancing mechanical strength and electrolysis performance in water electrolysis devices by forming stable ion conduction paths.

WO2024202656A1PCT designated stage expired Publication Date: 2024-10-03TOPPAN HOLDINGS INC

Patent Information

Application Number
PCT/JP2024/005335
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-02-15
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Membrane electrode assemblies in water electrolysis devices face issues with crack formation in the electrode catalyst layer, which impede the transfer of ions and electrons, reducing the performance and durability of the electrolysis process.

Method used

The use of an electrode catalyst layer comprising catalyst particles, an ionomer, and ionomer-adsorbing carbon fibers, where the ionomer-adsorptive carbon fibers adsorb the ionomer, and the layer includes hydrophilized vapor-grown carbon fibers to enhance mechanical strength and ion conductivity, or a coated fiber structure with a polymer containing Lewis acidic functional groups to improve adhesion and conductivity.

Benefits of technology

The proposed solutions significantly reduce crack formation, enhance mechanical properties, and improve electrolysis performance by forming a stable conduction path for ions, resulting in high durability and efficient water electrolysis.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024005335_03102024_PF_FP_ABST
    Figure JP2024005335_03102024_PF_FP_ABST
Patent Text Reader

Abstract

An electrode catalyst layer 2 comprises catalyst particles 12, an ionomer 13, and ionomer-adsorbing carbon fibers 14α. The ionomer-adsorbing carbon fibers 14α may have an ionomer adsorption amount of 10 mg or larger per g of the ionomer-adsorbing carbon fibers, may have a diameter within the range of 50 nm to 1 μm, and may be hydrophilized vapor-phase growth carbon fibers (VGCF).
Need to check novelty before this filing date? Find Prior Art

Description

Electrode catalyst layer and membrane electrode assembly

[0001] The present disclosure relates to an electrode catalyst layer and a membrane electrode assembly suitable for a water electrolysis device.

[0002] In recent years, there has been an accelerating trend toward using hydrogen as a primary energy source, as a CO2-free energy source that can be produced from various resources, in order to achieve carbon neutrality. Water electrolysis using renewable energy is seen as a promising method for producing such hydrogen. Generally, alkaline water electrolysis and proton exchange membrane (PEM) water electrolysis are known as water electrolysis methods. PEM water electrolysis in particular has attracted attention as a method that enables the miniaturization of water electrolysis equipment through highly efficient operation.

[0003] A PEM water electrolysis device generally includes a pair of main electrodes and a membrane electrode assembly provided between the pair of main electrodes. The membrane electrode assembly includes a stacked body in which an anode electrode catalyst layer is provided on one surface of a proton-conductive solid polymer electrolyte membrane, and a cathode electrode catalyst layer provided so as to sandwich the solid polymer electrolyte membrane together with the anode electrode catalyst layer.

[0004] When external power is applied to the anode and cathode electrode catalyst layers, a water electrolysis reaction occurs on the catalyst in each electrode catalyst layer. At the anode, protons, electrons, and oxygen are produced from water, and the protons travel through the solid polymer electrolyte membrane and the electrons travel through an external circuit to the cathode, where hydrogen is produced.

[0005] The membrane electrode assembly is obtained by forming an electrode catalyst layer on one surface of a solid polymer electrolyte membrane, for example, by a coating method (see, for example, Patent Document 1 listed below).

[0006] Alkaline water electrolysis can be easily scaled up but is poorly adaptable to fluctuations, while PEM water electrolysis has the disadvantage of being highly adaptable to fluctuations but using expensive precious metal materials. Therefore, anion exchange membrane (AEM) water electrolysis, which is expected to reduce material costs while maintaining the adaptability of PEM water electrolysis, has also attracted attention.

[0007] An AEM water electrolysis cell generally includes a pair of main electrodes and a membrane electrode assembly provided between the pair of main electrodes. The membrane electrode assembly includes a stack including an anode electrode catalyst layer provided on one surface of a solid polymer electrolyte membrane that conducts hydroxide ions, and a cathode electrode catalyst layer provided so as to sandwich the solid polymer electrolyte membrane together with the anode electrode catalyst layer.

[0008] When external electric power is applied to the anode-side electrode catalyst layer and the cathode-side electrode catalyst layer, the electrolysis reaction of water proceeds on the catalyst in each electrode catalyst layer, producing oxygen at the anode and hydrogen at the cathode.

[0009] The membrane electrode assembly is obtained by forming an electrode catalyst layer on one surface of a solid polymer electrolyte membrane, for example, by a coating method (see, for example, Patent Document 2 listed below).

[0010] JP 2019-83085 A International Publication No. 2017 / 159820

[0011] However, the membrane electrode assembly described in Patent Document 1 may suffer from cracks in the electrode catalyst layer, and there is room for improvement in terms of preventing cracks from occurring. The occurrence of cracks may inhibit the transfer of protons and electrons to the catalyst, resulting in a decrease in water electrolysis performance.

[0012] Furthermore, the membrane electrode assembly described in Patent Document 2 may suffer from cracks in the electrode catalyst layer, and there is room for improvement in terms of preventing cracks from occurring. The occurrence of cracks may inhibit the transfer of hydroxide ions and electrons to the catalyst, thereby reducing the water electrolysis performance.

[0013] The present disclosure has been made in view of the above-described problems, and aims to provide an electrode catalyst layer and a membrane electrode assembly that can suppress the occurrence of cracks in an electrode catalyst layer and are suitable for a water electrolysis device (water electrolysis cell) with improved water electrolysis performance.

[0014] [A1] An electrode catalyst layer comprising catalyst particles, an ionomer, and an ionomer-adsorbing carbon fiber capable of adsorbing the ionomer.

[0015] [A2] The electrode catalyst layer according to [A1], characterized in that the ionomer-adsorbing carbon fiber adsorbs the ionomer, and the amount of the ionomer adsorbed is 10 mg or more per 1 g of the ionomer-adsorbing carbon fiber.

[0016] [A3] The electrode catalyst layer according to [A1] or [A2], wherein the average fiber diameter of the ionomer-adsorbing carbon fibers is in the range of 50 nm or more and 1 μm or less.

[0017] [A4] The electrode catalyst layer according to any one of [A1] to [A3], wherein the ionomer-adsorbing carbon fiber is a hydrophilically treated carbon fiber.

[0018] [A5] The electrode catalyst layer according to any one of [A1] to [A4], wherein the ionomer-adsorbing carbon fiber is a vapor-grown carbon fiber (VGCF) that has been subjected to a hydrophilization treatment.

[0019] [A6] The electrode catalyst layer according to any one of [A1] to [A5], which is for a water electrolysis device.

[0020] [A7] The electrode catalyst layer according to any one of [A6], which is a cathode-side electrode catalyst layer.

[0021] [A8] A membrane electrode assembly comprising a polymer electrolyte membrane, and an anode-side electrode catalyst layer and a cathode-side electrode catalyst layer sandwiching the polymer electrolyte membrane, wherein at least one of the cathode-side electrode catalyst layer and the anode-side electrode catalyst layer is the electrode catalyst layer according to any one of [A1] to [A7].

[0022] [B1] An electrode catalyst layer comprising catalyst particles, a polymer electrolyte having hydroxide ion conductivity, and a coated fiber, wherein the coated fiber has a fiber core and a peripheral coating layer coating the peripheral surface of the fiber core, and the peripheral coating layer contains a polymer having a Lewis acidic functional group. [B2] The electrode catalyst layer according to [B1] or [B2], wherein the coated fiber has an intermediate coating layer between the fiber core and the peripheral coating layer, and the intermediate coating layer contains a polymer compound having a Lewis basic functional group. [B3] The electrode catalyst layer according to [B2], wherein the polymer compound of the intermediate coating layer has an azole structure. [B4] The electrode catalyst layer according to [B3], wherein the polymer compound of the intermediate coating layer is polybenzimidazole. [B5] The electrode catalyst layer according to any one of [B1] to [B4], wherein the fiber core is a conductive fiber. [B6] The electrode catalyst layer according to [B5], wherein the conductive fiber is a carbon fiber. [B7] The electrode catalyst layer according to [B6], wherein the carbon fiber is vapor-grown carbon fiber (VGCF). [B8] The electrode catalyst layer according to any one of [B1] to [B7], wherein the coated fiber has an average fiber diameter within a range of 0.1 to 1 μm. [B9] The electrode catalyst layer according to any one of [B1] to [B8], wherein the electrode catalyst layer is for an anion exchange membrane water electrolysis cell. [B10] The electrode catalyst layer according to [B9], wherein the electrode catalyst layer is a cathode-side electrode catalyst layer. [B11] A membrane / electrode assembly comprising a polymer electrolyte membrane, and an anode-side electrode catalyst layer and a cathode-side electrode catalyst layer sandwiching the polymer electrolyte membrane, wherein the cathode-side electrode catalyst layer is the electrode catalyst layer according to any one of [B1] to [B10].

[0023] According to the electrode catalyst layer and membrane electrode assembly of one embodiment of the present invention, a laminate for a water electrolysis cell having sufficient mechanical strength and improved water electrolysis performance can be provided using a simple method.

[0024] 1 is an exploded perspective view schematically showing a membrane electrode assembly having an electrode catalyst layer for a water electrolysis cell according to one embodiment of the present invention; 2 is a cross-sectional schematic view of a cathode-side electrode catalyst layer according to one embodiment of the present invention; 3 is a cross-sectional view taken along the axis of a coated fiber according to one embodiment of the present invention; 4 is a cross-sectional view of an embodiment of a water electrolysis device according to the present disclosure;

[0025] <Embodiment A> Hereinafter, an embodiment of the present invention will be described with reference to the accompanying drawings. The drawings are schematic, and the relationship between thickness and planar dimensions, the thickness ratio of each layer, and the like differ from the actual ones. Furthermore, the embodiments shown below exemplify configurations for embodying the technical concept of the present invention, and the technical concept of the present invention is not limited to the materials, shapes, structures, and the like of the components described below. The technical concept of the present invention can be modified in various ways within the technical scope defined by the claims.

[0026] [Membrane Electrode Assembly] As shown in FIG. 1 , the membrane electrode assembly 11 of this embodiment includes a polymer electrolyte membrane 1, an anode-side electrode catalyst layer 3 (shown on the lower side in FIG. 1 ) that sandwiches the polymer electrolyte membrane 1 from above and below, and a cathode-side electrode catalyst layer 2 (shown on the upper side in FIG. 1 ).

[0027] (Cathode-Side Electrode Catalyst Layer 2) As shown in FIG. 2, the cathode-side electrode catalyst layer 2 includes catalyst particles 12, an ionomer (polymer electrolyte) 13, and ionomer-adsorbing carbon fibers 14α.

[0028] (Cathode-side catalyst particles) The catalyst particles 12 are particulate. When improved activity of the catalyst particles is required, the average particle size of the catalyst particles is preferably 20 nm or less, and more preferably 5 nm or less. When stable activity of the catalyst particles is required, the average particle size of the catalyst particles is preferably 0.5 nm or more, and more preferably 1 nm or more.

[0029] The catalyst particles in the cathode-side electrode catalyst layer are catalysts for carrying out reduction reactions. Platinum group elements, metals, alloys, oxides, and double oxides of these metals can be used as constituent materials of the catalyst particles. Examples of platinum group elements include platinum, palladium, ruthenium, iridium, rhodium, and osmium, and examples of metals include iron, lead, copper, chromium, cobalt, nickel, manganese, vanadium, molybdenum, gallium, and aluminum. The double oxide referred to here is an oxide made of two types of metals.

[0030] The catalyst particles of the cathode-side electrode catalyst layer may be supported on a support 15. The support is a particle that is conductive and not eroded by the catalyst material. An example of the support is carbon particles. When an expansion of the electron conduction path is required, the particle size of the support is preferably 10 nm or more. When a reduction in the resistance value of the electrode catalyst layer is required or an increase in the amount of catalyst particles supported is required, the particle size of the support is preferably 1000 nm or less, and more preferably 100 nm or less. An example of a constituent material of the support is at least one selected from the group consisting of carbon black, graphite, activated carbon, and fullerene. The carbon black is at least one selected from the group consisting of acetylene black, furnace black, and ketjen black.

[0031] (Ionomer (Polymer Electrolyte)) The ionomer (polymer electrolyte) 13 is a polymer electrolyte having proton or hydroxide ion conductivity. The proton-conductive polymer electrolyte has, for example, a particulate shape or a shape in which a plurality of particles are united. An example of a proton-conductive polymer electrolyte is a fluorine-based polymer electrolyte or a hydrocarbon-based polymer electrolyte. An example of a fluorine-based polymer electrolyte is at least one selected from the group consisting of Nafion (registered trademark, manufactured by DuPont), Flemion (registered trademark, manufactured by Asahi Glass Co., Ltd.), Aciplex (registered trademark, manufactured by Asahi Kasei Corporation), and Gore-Select (registered trademark, manufactured by Gore Japan LLC). An example of a hydrocarbon-based cation exchange electrolyte is at least one selected from the group consisting of sulfonated polyether ketone, sulfonated polyether sulfone, sulfonated polyether ether sulfone, sulfonated polysulfide, and sulfonated polyphenylene. The polymer electrolyte having hydroxide ion conductivity is not particularly limited as long as it conducts hydroxide ions. For example, there are fluorine-based anion exchange electrolytes and hydrocarbon-based anion exchange electrolytes. Examples of fluorine-based electrolytes include perfluorocarbon-based electrolytes, and examples of hydrocarbon-based electrolytes include styrene-based electrolytes and acrylic-based electrolytes.

[0032] (Ionomer-adsorbing carbon fiber 14α) The ionomer-adsorbing carbon fiber 14α can adsorb an ionomer. There are no particular limitations on the ionomer-adsorbing carbon fiber, but it may be a carbon fiber to which hydrophilicity has been imparted (hydrophilized carbon fiber). For example, hydrophilized carbon fiber manufactured to have hydrophilic properties, or hydrophilized carbon fiber obtained by treating non-hydrophilic carbon fiber to impart hydrophilic properties can be used. Examples of treatments to impart hydrophilic properties to carbon fibers include ozone treatment, oxygen plasma treatment, electrolytic oxidation treatment, and mixed acid treatment.

[0033] The type of carbon fiber having ionomer adsorption is not particularly limited, and may be selected from carbon fibers such as carbon fibers, carbon nanofibers, carbon nanotubes, and carbon nanohorns. That is, the ionomer adsorbent carbon fiber may be solid or hollow. Among them, vapor-grown carbon fiber (VGCF) is preferred.

[0034] The amount of ionomer adsorbed by the ionomer-adsorbing carbon fiber 14α is preferably 10 mg or more per 1 g of the ionomer-adsorbing carbon fiber.

[0035] In the ionomer-adsorbing carbon fiber 14α, the ionomer (polymer electrolyte) is adsorbed onto the surface of the carbon fiber, which improves the mechanical properties of the electrode catalyst layer and improves durability, such as by suppressing the occurrence of cracks in the electrode catalyst layer. In addition to the improvement in mechanical properties, the adsorption of the ionomer (polymer electrolyte) onto the ionomer-adsorbing carbon fiber 14α forms a conduction path for protons or hydroxide ions, resulting in high electrolysis performance.

[0036] On the other hand, if the surface of the carbon fiber is not ionomer-adsorbent, it is difficult for the ionomer (polymer electrolyte) to adsorb. As a result, the mechanical properties of the electrode catalyst layer are insufficient, making it difficult to suppress cracking, and it is presumed that durability cannot be improved. Furthermore, it is presumed that the dispersion of the ionomer inhibits the formation of conduction paths for protons or hydroxide ions, making it impossible to improve electrolysis performance.

[0037] The average fiber diameter of the ionomer-adsorbing carbon fiber 14α is not particularly limited, but is preferably 50 nm to 1 μm, and more preferably 0.1 to 0.4 μm. In this case, the occurrence of cracks in the electrode catalyst layer is more likely to be suppressed. Furthermore, the adhesion between the polymer electrolyte membrane and the electrode catalyst layer can be improved. This can suppress the occurrence of voids due to peeling between the polymer electrolyte membrane and the electrode catalyst layer, and further suppress the increase in resistance of the membrane electrode assembly caused by these voids. It is estimated that if the average fiber diameter of the ionomer-adsorbing carbon fiber is less than 50 nm, it may be difficult to improve the mechanical properties. It is also estimated that if the average fiber diameter of the ionomer-adsorbing carbon fiber is greater than 1 μm, it may not be possible to disperse the ionomer-adsorbing carbon fiber as an ink.

[0038] The average fiber diameter refers to the average diameter measured for the cross section of the exposed ionomer-adsorbed carbon fiber when the cross section of the electrode catalyst layer is observed using a scanning electron microscope (SEM). When the ionomer-adsorbed carbon fiber is cut obliquely to its major axis, an elliptical cross section is obtained. In this case, the diameter refers to the diameter of a perfect circle fitted along the minor axis of the ellipse. Furthermore, when the cross section of the electrode catalyst layer is observed using an SEM, the surface of the ionomer-adsorbed carbon fiber may be exposed rather than the cross section of the ionomer-adsorbed carbon fiber. In this case, the diameter refers to the width of the fiber perpendicular to the major axis of the exposed ionomer-adsorbed carbon fiber. The average fiber diameter of the ionomer-adsorbed carbon fiber refers to the arithmetic mean value of fiber diameters obtained by similar measurements at at least 20 observation points.

[0039] As a method for exposing the cross section of the electrode catalyst layer, known methods such as ion milling and ultramicrotome can be used.

[0040] The average fiber length of the ionomer-adsorbing carbon fiber is not particularly limited, but is preferably 500 nm or more, more preferably 1 μm or more. In this case, the ionomer-adsorbing carbon fiber becomes entangled, forming pores of appropriate size in the electrode catalyst layer, and improving the mechanical properties of the electrode catalyst layer. However, the average fiber length of the ionomer-adsorbing carbon fiber is preferably 100 μm or less, more preferably 40 μm or less.

[0041] The average fiber length of the ionomer-adsorbed carbon fibers refers to the arithmetic mean value of the fiber lengths obtained by measuring the lengths of at least 10 ionomer-adsorbed carbon fibers. The average fiber length of the ionomer-adsorbed carbon fibers in the electrode catalyst layer can be determined by measuring the particle size distribution using a solution in which the electrode catalyst layer is dissolved in a solvent. Specifically, the correlation between the average fiber length determined using an electron microscope and the peak position in the particle size distribution measurement is determined in advance, and the average fiber length of the ionomer-adsorbed carbon fibers in the electrode catalyst layer is determined based on this correlation and the peak position determined by the particle size distribution measurement.

[0042] The composition of the cathode-side electrode catalyst layer 2 is not particularly limited, but the mass of the ionomer (polymer electrolyte) (solid content) can be 0.1 to 0.4, and the mass of the ionomer-adsorbing carbon fiber can be 0.025 to 0.25, assuming that the mass of the catalyst particles is 1.

[0043] 2 , the anode-side electrode catalyst layer 3 contains catalyst particles 22 and an ionomer (polymer electrolyte) 23. When the anode-side electrode catalyst layer 3 contains the ionomer-adsorbing carbon fibers 14α, as in the cathode-side electrode catalyst layer 2, the mechanical properties of the electrode catalyst layer are improved, resulting in improved durability. In addition to the improved mechanical properties, the polymer electrolyte is adsorbed onto the ionomer-adsorbing carbon fibers 14α, forming a conduction path for protons or hydroxide ions, thereby achieving high electrolysis performance.

[0044] (Catalyst Particles) The catalyst particles 22 are particulate. When improved activity of the catalyst particles is required, the average particle size of the catalyst particles is preferably 20 nm or less, and more preferably 5 nm or less. When stabilization of the activity of the catalyst particles is required, the average particle size of the catalyst particles is preferably 0.5 nm or more, and more preferably 1 nm or more.

[0045] The catalyst particles in the anode-side electrode catalyst layer are catalysts for carrying out oxidation reactions. The constituent materials of the catalyst particles can be metals included in the platinum group, metals other than the platinum group, or alloys, oxides, double oxides, and carbides thereof. Among these, ruthenium, rhodium, palladium, iridium, platinum, and alloys containing at least one of these metals are preferred due to their high catalytic activity. The catalyst particles may be composed of only one of the above-mentioned examples, or a combination of two or more of them.

[0046] The catalyst particles of the anode-side electrode catalyst layer may be supported on a carrier 25. The carrier is a particle that is conductive and is not eroded in an oxidizing atmosphere. An example of the carrier is an oxide particle containing titanium, tin, or zirconium. When an expansion of the electron conduction path is required, the particle size of the carrier is preferably 10 nm or more. When a reduction in the resistance value of the electrode catalyst layer or an increase in the amount of catalyst particles supported is required, the particle size of the carrier is preferably 1000 nm or less, and more preferably 100 nm or less.

[0047] (Ionomer (Polymer Electrolyte)) The ionomer (polymer electrolyte) 23 on the anode side can be the same as the ionomer (polymer electrolyte) on the cathode side.

[0048] The composition of the anode-side electrode catalyst layer 3 is not particularly limited, but the mass of the ionomer (polymer electrolyte) (solid content) can be set to 0.1 to 0.4, and the mass of the ionomer-adsorbing carbon fiber can be set to 0.025 to 0.25, assuming that the mass of the catalyst particles is 1.

[0049] (Polymer electrolyte membrane 1) A fluorine-based polymer electrolyte membrane or a hydrocarbon-based polymer electrolyte membrane having proton or hydroxide ion conductivity is an example of the polymer electrolyte membrane 1. The polymer electrolyte membrane is not particularly limited as long as it conducts protons or hydroxide ions.

[0050] An example of a fluorine-based polymer electrolyte membrane having proton conductivity is at least one selected from the group consisting of Nafion (registered trademark, manufactured by DuPont Co., Ltd.), Flemion (registered trademark, manufactured by Asahi Glass Co., Ltd.), Aciplex (registered trademark, manufactured by Asahi Kasei Corporation), and Gore-Select (registered trademark, manufactured by Gore Japan LLC). An example of a constituent material of a hydrocarbon-based polymer electrolyte membrane having proton conductivity is at least one selected from the group consisting of sulfonated polyether ketone, sulfonated polyether sulfone, sulfonated polyether ether sulfone, sulfonated polysulfide, and sulfonated polyphenylene.

[0051] An example of a fluorine-based anion exchange electrolyte membrane having hydroxide ion conductivity is a perfluorocarbon-based electrolyte membrane, while an example of a hydrocarbon-based anion exchange electrolyte membrane is a styrene-based electrolyte membrane or an acrylic-based electrolyte membrane.

[0052] When it is required to improve the adhesion between the electrode catalyst layer and the polymer electrolyte membrane, if the constituent material of the polymer electrolyte of the electrode is a fluorine-based polymer electrolyte, it is preferable that the constituent material of the polymer electrolyte membrane is also a fluorine-based polymer electrolyte. Also, if the constituent material of the polymer electrolyte of the electrode is a hydrocarbon-based polymer electrolyte, it is preferable that the constituent material of the polymer electrolyte membrane is also a hydrocarbon-based polymer electrolyte. Furthermore, it is preferable that the constituent material of the polymer electrolyte membrane is the same as the constituent material of the polymer electrolyte of the electrode.

[0053] [Method for Manufacturing Membrane Electrode Assembly] Next, an example of a method for manufacturing the membrane electrode assembly having the above-described configuration will be described.

[0054] The membrane electrode assembly is produced by a method including the following first to third steps.

[0055] The first step is a step of producing ionomer-adsorbing carbon fibers by subjecting carbon fibers to oxygen plasma treatment to impart hydrophilic properties to the surfaces of the carbon fibers.

[0056] The second step is a step of producing a cathode-side catalyst ink containing catalyst particles, an ionomer (polymer electrolyte), the ionomer-adsorbing carbon fiber obtained in the first step, and a solvent, and the other step is a step of producing an anode-side catalyst ink containing catalyst particles, an ionomer (polymer electrolyte), and a solvent, in which the ionomer can be adsorbed onto the ionomer-adsorbing carbon fiber.

[0057] The third step is a step of applying the cathode-side catalyst ink and the anode-side catalyst ink obtained in the second step onto a polymer electrolyte membrane and drying the solvent, thereby forming a cathode-side electrode catalyst layer and an anode-side electrode catalyst layer on both sides of the polymer electrolyte membrane.

[0058] [Detailed Description] (First Step) In the first step, the surface of the carbon fiber is subjected to a treatment such as oxygen plasma treatment to impart hydrophilicity to the surface of the carbon fiber, thereby producing an ionomer-adsorbing carbon fiber. The degree of hydrophilicity imparted to the surface of the carbon fiber, in other words, the degree of ionomer adsorption, can be adjusted by adjusting the time for which the carbon fiber is subjected to the hydrophilization treatment such as oxygen plasma treatment. The amount of ionomer adsorbed to the obtained ionomer-adsorbing carbon fiber can be calculated by contacting the carbon fiber with a dispersion in which a predetermined concentration of ionomer is dispersed, filtering the dispersion with a predetermined filter (e.g., 0.3 to 0.5 μm diameter), and measuring the concentration of ionomer contained in the filtrate.

[0059] (Second Step) A cathode-side catalyst ink can be produced by mixing catalyst particles, an ionomer (polymer electrolyte), the ionomer-adsorbing carbon fiber obtained in the first step, and a solvent. An anode-side catalyst ink can also be produced in the same manner. The solvent constituting the catalyst ink does not corrode the catalyst particles, the ionomer (polymer electrolyte), and the ionomer-adsorbing carbon fiber, and dissolves the ionomer (polymer electrolyte) or disperses it as a fine gel. An example of the solvent constituting the catalyst ink is at least one selected from the group consisting of alcohols, ketone-based solvents, ether-based solvents, and polar solvents. An example of the alcohol is at least one selected from the group consisting of methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, isobutyl alcohol, tert-butyl alcohol, and pentanol. An example of a ketone-based solvent is at least one selected from the group consisting of acetone, methyl ethyl ketone, pentanone, methyl isobutyl ketone, heptanone, cyclohexanone, methylcyclohexanone, acetonylacetone, and diisobutyl ketone. An example of an ether-based solvent is at least one selected from the group consisting of tetrahydrofuran, dioxane, diethylene glycol dimethyl ether, anisole, methoxytoluene, and dibutyl ether. An example of a polar solvent is at least one selected from the group consisting of dimethylformamide, dimethylacetamide, N-methylpyrrolidone, ethylene glycol, diethylene glycol, diacetone alcohol, and 1-methoxy-2-propanol. The solvent constituting the catalyst ink may contain water, which has a high affinity for the polymer electrolyte.

[0060] When improved dispersibility of catalyst particles is required, the catalyst ink preferably contains a dispersant. Examples of dispersants include anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants. When improved dispersibility of the catalyst ink is required, a dispersion treatment is preferably performed in the production of the catalyst ink. Examples of dispersion treatments include stirring with a ball mill and a roll mill, stirring with a shear mill, stirring with a wet mill, stirring by applying ultrasonic waves, and stirring with a homogenizer.

[0061] When suppression of cracking on the surface of the electrode catalyst layer is required, the solid content of the catalyst ink is preferably 50% by mass or less.When an improvement in the film formation rate of the electrode catalyst layer is required, the solid content of the catalyst ink is preferably 1% by mass or more.

[0062] (Step 3) Examples of methods for applying the catalyst ink onto a substrate include a doctor blade method, a dipping method, a screen printing method, and a roll coating method. The substrate to which the catalyst ink is applied is a transfer sheet. Examples of materials constituting the transfer sheet include fluorine-based resins and organic polymer compounds other than fluorine-based resins. Examples of fluorine-based resins include ethylene tetrafluoroethylene copolymer (ETFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroperfluoroalkylvinyl ether copolymer (PFA), and polytetrafluoroethylene (PTFE). Examples of organic polymer compounds include polyimide, polyethylene terephthalate, polyamide, polysulfone, polyethersulfone, polyphenylene sulfide, polyether ether ketone, polyetherimide, polyarylate, and polyethylene naphthalate.

[0063] In the above embodiment, the ionomer-adsorbing carbon fiber is provided in the electrode catalyst layer on the cathode side, but it can also be provided in the electrode catalyst layer on the anode side.

[0064] Hereinafter, the electrode catalyst layer and membrane electrode assembly for a water electrolysis apparatus according to this embodiment will be described with reference to specific examples and comparative examples, but this embodiment is not limited to the following examples and comparative examples.

[0065] <Effects and Others> According to this embodiment, it is possible to manufacture a membrane electrode assembly for a water electrolysis system having an electrode catalyst layer with high mechanical properties and excellent electrolysis performance and durability, without using complicated processes.

[0066] Example A1 Production of Ionomer-Adsorbing Carbon Fiber Carbon fibers having an average fiber diameter of 150 nm (VGCF-H (registered trademark), vapor-grown carbon fibers manufactured by Showa Denko K.K.) were subjected to a hydrophilization treatment using oxygen plasma to obtain ionomer-adsorbing carbon fibers. When a fluorine-based polymer electrolyte (Nafion (registered trademark) dispersion) was used as the proton-conductive ionomer, the ionomer-adsorbing carbon fibers of Example A1 were confirmed to have an ionomer adsorption amount of 10 mg or more per 1 g of the ionomer-adsorbing carbon fibers.

[0067] [Production of Cathode-Side Catalyst Ink] The catalyst particles, ionomer, and ionomer-adsorbing carbon fiber shown below were mixed in a solvent and dispersed for 30 minutes using a planetary ball mill to produce a catalyst ink. A mixed solvent of ultrapure water and 1-propanol was used as the solvent for the catalyst ink. The volume ratio of ultrapure water to 1-propanol was 1:1. The catalyst ink was adjusted so that the solid content in the catalyst ink was 10% by mass. Catalyst particles: Pt-supported carbon particles Ionomer: Fluorine-based polymer electrolyte (Nafion (registered trademark) dispersion) Blending ratio: The catalyst ink had a mass of catalyst particles of 1, a mass of ionomer (solids) of 0.4, and a mass of ionomer-adsorbing carbon fiber of 0.05.

[0068] [Production of Anode-Side Catalyst Ink] The catalyst particles and ionomer shown below were mixed in a solvent and dispersed for 30 minutes using a planetary ball mill to produce a catalyst ink. A mixed solvent of ultrapure water and 1-propanol was used as the solvent for the catalyst ink. The volume ratio of ultrapure water to 1-propanol was 1:1. The catalyst ink was adjusted so that the solid content in the catalyst ink was 10% by mass. - Catalyst particles: iridium oxide - Ionomer: fluorine-based polymer electrolyte (Nafion (registered trademark) dispersion) - Blending ratio: The mass of the catalyst particles in the catalyst ink was 1, and the mass of the ionomer (solid content) was 0.2.

[0069] [Fabrication of Membrane Electrode Assembly] The prepared cathode catalyst ink was applied to one side of a proton-conductive polymer electrolyte membrane (fluorine-based polymer electrolyte membrane) using a die coater to form a rectangular coating film measuring 50 mm long x 50 mm wide. The amount of the cathode catalyst ink applied was 0.5 mg / cm. 2 The amount of the anode catalyst ink was adjusted so that the catalyst was 0.5 mg / cm. The anode catalyst ink was then dried in an oven to volatilize the dispersion medium contained in the coating film, thereby forming a cathode-side electrode catalyst layer. Next, the prepared anode catalyst ink was applied to the surface of the polymer electrolyte membrane opposite to the surface on which the cathode-side electrode catalyst layer was formed, thereby forming a rectangular coating film measuring 50 mm long x 50 mm wide. The amount of the anode catalyst ink applied was such that the catalyst was 0.5 mg / cm. 2 The coating was dried in an oven to volatilize the dispersion medium contained in the coating, thereby forming an anode-side electrode catalyst layer, thereby obtaining a membrane electrode assembly. Both electrode catalyst layers in Example A1 were free from cracks and did not peel off from the polymer electrolyte membrane.

[0070] Example A2 A membrane electrode assembly of Example A2 was obtained using the same procedure as in Example A1, except that carbon fibers with an average fiber diameter of 0.8 μm were used as the carbon fibers in the ionomer-adsorbing carbon fibers. When a fluorine-based polymer electrolyte (Nafion (registered trademark) dispersion) was used as the proton-conductive ionomer, the ionomer-adsorbing carbon fibers of Example A2 were confirmed to have an ionomer adsorption amount of 10 mg or more per 1 g of the ionomer-adsorbing carbon fibers. Both electrode catalyst layers of Example A2 were free of cracks and did not peel off from the polymer electrolyte membrane.

[0071] Example A3 Production of Ionomer-Adsorbing Carbon Fiber Carbon fibers with an average fiber diameter of 150 nm (VGCF-H (registered trademark), vapor-grown carbon fibers manufactured by Showa Denko K.K.) were subjected to a hydrophilization treatment using oxygen plasma to obtain ionomer-adsorbing carbon fibers. When a hydrocarbon-based anion-exchange electrolyte was used as the ionomer having hydroxide ion conductivity, the ionomer-adsorbing carbon fiber of Example A3 was confirmed to have an ionomer adsorption amount of 10 mg or more per 1 g of the ionomer-adsorbing carbon fiber.

[0072] [Production of Cathode-Side Catalyst Ink] The catalyst particles, ionomer, and ionomer-adsorbing carbon fiber shown below were mixed in a solvent and dispersed for 30 minutes using a planetary ball mill to produce a catalyst ink. A mixed solvent of ultrapure water and 1-propanol was used as the solvent for the catalyst ink. The volume ratio of ultrapure water to 1-propanol was 1:1. The catalyst ink was adjusted so that the solid content in the catalyst ink was 10% by mass. Catalyst particles: Pt-supported carbon particles Ionomer: hydrocarbon-based anion exchange electrolyte Blending ratio: The catalyst ink had a mass of catalyst particles of 1, a mass of ionomer (solids) of 0.3, and a mass of ionomer-adsorbing carbon fiber of 0.05.

[0073] [Production of anode-side catalyst ink] The catalyst particles and ionomer shown below were mixed in a solvent and dispersed for 30 minutes using a planetary ball mill to produce a catalyst ink. A mixed solvent of ultrapure water and 1-propanol was used as the solvent for the catalyst ink. The volume ratio of ultrapure water to 1-propanol was 1:1. The catalyst ink was adjusted so that the solid content in the catalyst ink was 10% by mass. - Catalyst particles: iridium oxide - Ionomer: hydrocarbon-based anion exchange electrolyte - Blending ratio: The mass of the catalyst particles in the catalyst ink was 1, and the mass of the ionomer (solids) was 0.3.

[0074] [Fabrication of Membrane Electrode Assembly] The prepared cathode catalyst ink was applied to one side of a polymer electrolyte membrane (hydrocarbon-based anion-exchange electrolyte membrane) having hydroxide ion conductivity using a die coater to form a rectangular coating film measuring 50 mm long x 50 mm wide. The amount of the cathode catalyst ink applied was 0.5 mg / cm. 2 The amount of the anode catalyst ink was adjusted so that the catalyst was 0.5 mg / cm. The anode catalyst ink was then dried in an oven to volatilize the dispersion medium contained in the coating film, thereby forming a cathode-side electrode catalyst layer. Next, the prepared anode catalyst ink was applied to the surface of the polymer electrolyte membrane opposite to the surface on which the cathode-side electrode catalyst layer was formed, thereby forming a rectangular coating film measuring 50 mm long x 50 mm wide. The amount of the anode catalyst ink applied was such that the catalyst was 0.5 mg / cm. 2 The coating was dried in an oven to volatilize the dispersion medium contained in the coating, thereby forming an anode-side electrode catalyst layer, thereby obtaining a membrane electrode assembly. Both electrode catalyst layers in Example A3 were free from cracks and did not peel off from the polymer electrolyte membrane.

[0075] Example A4 A membrane electrode assembly of Example A4 was obtained using the same procedure as in Example A3, except that carbon fibers with an average fiber diameter of 0.8 μm were used as the carbon fibers in the ionomer-adsorbing carbon fibers. When a hydrocarbon-based anion-exchange electrolyte was used as the ionomer with hydroxide ion conductivity, the ionomer-adsorbing carbon fibers of Example A4 were confirmed to have an ionomer adsorption amount of 10 mg or more per 1 g of the ionomer-adsorbing carbon fibers. Both electrode catalyst layers of Example A4 were free of cracks and did not peel off from the polymer electrolyte membrane.

[0076] Comparative Example A1 A membrane electrode assembly of Comparative Example A1 was obtained in the same manner as in Example A1, except that carbon fibers (VGCF-H (registered trademark), vapor-grown carbon fibers manufactured by Showa Denko K.K.) having an average fiber diameter of 150 nm were used instead of the ionomer-adsorbing carbon fibers without being subjected to a hydrophilization treatment. When a fluorine-based polymer electrolyte (Nafion (registered trademark) dispersion) was used as the ionomer having proton conductivity, it was confirmed that the carbon fibers of Comparative Example A1 had an ionomer adsorption amount of less than 10 mg per 1 g of carbon fibers.

[0077] In Comparative Example A1, no cracks were observed during the formation of the cathode-side electrode catalyst layer, and no peeling from the polymer electrolyte membrane occurred. However, cracks occurred in the cathode-side electrode catalyst layer during the formation of the anode-side electrode catalyst layer, and partial peeling from the polymer electrolyte membrane was observed.

[0078] Comparative Example A2 A membrane electrode assembly of Comparative Example A2 was obtained in the same manner as in Example A2, except that carbon fibers having an average fiber diameter of 0.8 μm were used without hydrophilization treatment instead of the ionomer-adsorbing carbon fibers. When a fluorine-based polymer electrolyte (Nafion (registered trademark) dispersion) was used as the ionomer having proton conductivity, it was confirmed that the carbon fibers of Comparative Example A2 had an ionomer adsorption amount of less than 10 mg per 1 g of carbon fibers.

[0079] In Comparative Example A2, no cracks were observed during the formation of the cathode-side electrode catalyst layer, and no peeling from the polymer electrolyte membrane occurred. However, cracks occurred in the cathode-side electrode catalyst layer during the formation of the anode-side electrode catalyst layer, and partial peeling from the polymer electrolyte membrane was observed.

[0080] Comparative Example A3: A membrane electrode assembly of Comparative Example A3 was obtained using the same procedure as in Example A1, except that ionomer-adsorbing carbon fiber was not used. Significant cracking occurred during the formation of the cathode-side electrode catalyst layer of Comparative Example A3, and significant peeling from the polymer electrolyte membrane was observed. Therefore, it was not possible to apply the anode-side catalyst ink.

[0081] Comparative Example A4 A membrane / electrode assembly of Comparative Example A4 was obtained in the same manner as in Example A3, except that carbon fibers (VGCF-H (registered trademark), vapor-grown carbon fibers manufactured by Showa Denko K.K.) having an average fiber diameter of 150 nm were used instead of the ionomer-adsorbing carbon fibers without being subjected to a hydrophilization treatment. When a hydrocarbon-based anion-exchange electrolyte was used as the ionomer having hydroxide ion conductivity, it was confirmed that the carbon fibers of Comparative Example A4 had an ionomer adsorption amount of less than 10 mg per 1 g of carbon fibers.

[0082] In Comparative Example A4, no cracks were observed during the formation of the cathode-side electrode catalyst layer, and no peeling from the polymer electrolyte membrane occurred. However, cracks occurred in the cathode-side electrode catalyst layer during the formation of the anode-side electrode catalyst layer, and partial peeling from the polymer electrolyte membrane was observed.

[0083] Comparative Example A5 A membrane electrode assembly of Comparative Example A5 was obtained in the same manner as in Example A4, except that carbon fibers having an average fiber diameter of 0.8 μm were used instead of the ionomer-adsorbing carbon fibers without being subjected to hydrophilization treatment. When a hydrocarbon-based anion exchange electrolyte was used as the ionomer having hydroxide ion conductivity, it was confirmed that the carbon fibers of Comparative Example A5 had an ionomer adsorption amount of less than 10 mg per 1 g of carbon fibers.

[0084] In Comparative Example A5, no cracks were observed during the formation of the cathode-side electrode catalyst layer, and no peeling from the polymer electrolyte membrane occurred. However, cracks occurred in the cathode-side electrode catalyst layer during the formation of the anode-side electrode catalyst layer, and partial peeling from the polymer electrolyte membrane was observed.

[0085] Comparative Example A6: A membrane electrode assembly of Comparative Example A6 was obtained using the same procedure as in Example A3, except that ionomer-adsorbing carbon fiber was not used. Significant cracking occurred during the formation of the cathode-side electrode catalyst layer of Comparative Example A6, and significant peeling from the polymer electrolyte membrane was observed. Therefore, it was not possible to apply the anode-side catalyst ink.

[0086] When the membrane electrode assemblies obtained in Examples A1 to A4, Comparative Examples A1 to A2, and Comparative Examples A4 to A5 were immersed in water, both electrode catalyst layers in Examples A1 to A2 did not peel off from the polymer electrolyte membrane, but the cathode-side electrode catalyst layer in Comparative Examples A1 to A2 and A4 to A5 peeled off from the polymer electrolyte membrane. Furthermore, when the water electrolysis performance was evaluated using each membrane electrode assembly, the membrane electrode assemblies obtained in Examples A1 to A2 exhibited good electrolysis performance, but the membrane electrode assemblies obtained in Comparative Examples A1 to A2 and A4 to A5 exhibited significantly reduced electrolysis performance after repeated electrolysis. The electrolysis performance results for the membrane electrode assemblies prepared in the Examples and Comparative Examples confirmed that the membrane electrode assemblies prepared in the Examples had sufficient adhesion strength between the cathode-side electrode catalyst layer and the electrolyte membrane, and good electrolysis performance was obtained.

[0087] <Embodiment B> An embodiment of the present invention will be described below with reference to the accompanying drawings. The drawings are schematic, and the relationship between thickness and planar dimensions, the thickness ratio of each layer, and the like differ from the actual ones. Furthermore, the embodiments shown below exemplify configurations for embodying the technical concept of the present invention, and the technical concept of the present invention is not limited to the materials, shapes, structures, and the like of the components described below. The technical concept of the present invention can be modified in various ways within the technical scope defined by the claims.

[0088] [Membrane Electrode Assembly] As shown in FIG. 1 , the membrane electrode assembly 11 of this embodiment includes a polymer electrolyte membrane 1, an anode electrode catalyst layer 3 (shown on the upper side in FIG. 1 ) that sandwiches the polymer electrolyte membrane 1 from above and below, and a cathode electrode catalyst layer 2 (shown on the lower side in FIG. 1 ).

[0089] (Cathode-Side Electrode Catalyst Layer 2) As shown in FIG. 2, the cathode-side electrode catalyst layer 2 includes catalyst particles 12, a polymer electrolyte 13, and coated fibers .

[0090] (Catalyst Particles) The catalyst particles 12 are particulate. When improved activity of the catalyst particles is required, the average particle size of the catalyst particles is preferably 20 nm or less, and more preferably 5 nm or less. When stabilization of the activity of the catalyst particles is required, the average particle size of the catalyst particles is preferably 0.5 nm or more, and more preferably 1 nm or more.

[0091] The catalyst particles in the cathode-side electrode catalyst layer are catalysts for carrying out reduction reactions. Platinum group elements, metals, alloys, oxides, and double oxides of these metals can be used as constituent materials of the catalyst particles. Examples of platinum group elements include platinum, palladium, ruthenium, iridium, rhodium, and osmium, and examples of metals include iron, lead, copper, chromium, cobalt, nickel, manganese, vanadium, molybdenum, gallium, and aluminum. The double oxide referred to here is an oxide made of two types of metals.

[0092] The catalyst particles of the cathode-side electrode catalyst layer may be supported on a support 15. The support is a particle that is conductive and not eroded by the catalyst material. An example of the support is carbon particles. When an expansion of the electron conduction path is required, the particle size of the support is preferably 10 nm or more. When a reduction in the resistance value of the electrode catalyst layer is required or an increase in the amount of catalyst particles supported is required, the particle size of the support is preferably 1000 nm or less, and more preferably 100 nm or less. An example of a constituent material of the support is at least one selected from the group consisting of carbon black, graphite, activated carbon, and fullerene. The carbon black is at least one selected from the group consisting of acetylene black, furnace black, and ketjen black.

[0093] (Polymer Electrolyte) The polymer electrolyte 13 is a polymer electrolyte having hydroxide ion conductivity, and is a so-called anion exchange membrane. The polymer electrolyte is not particularly limited as long as it conducts hydroxide ions. For example, there are fluorine-based anion exchange electrolytes and hydrocarbon-based anion exchange electrolytes. Examples of fluorine-based electrolytes include perfluorocarbon-based electrolytes, and examples of hydrocarbon-based electrolytes include styrene-based electrolytes and acrylic-based electrolytes.

[0094] 3, the coated fiber 14 has a fiber core 14A and an outer coating layer 14C that coats the outer surface of the fiber core 14A. It is preferable to have an intermediate coating layer 14B between the fiber core 14A and the outer coating layer 14C.

[0095] (Fiber core 14A) The fiber core 14A is not particularly limited and may be a non-conductive fiber, but is preferably a conductive fiber. Examples of non-conductive fibers include polymer fibers obtained by electrospinning and cellulose nanofibers. Examples of conductive fibers include carbon fibers such as carbon fibers, carbon nanotubes, and carbon nanohorns, and conductive polymer nanofibers. In other words, the fiber core may be solid or hollow.

[0096] Among conductive fiber cores, the fiber core 14A is preferably a carbon fiber, and particularly preferably a vapor-grown carbon fiber (VGCF). The average fiber diameter of the fiber core may be 45 nm to 0.8 μm. The average fiber diameter of the fiber core can be measured in the same manner as the average fiber diameter of the coated fiber.

[0097] (Outer Coating Layer 14C) The outer coating layer 14C contains a polymer having a Lewis acidic functional group in its molecular structure. The Lewis acidic functional group refers to a functional group capable of accepting an electron pair. The Lewis acidic functional group may be a functional group capable of donating a proton. An example of the Lewis acidic functional group is —SO 3The functional groups are —H and —COOH. An example of a polymer containing a Lewis acid functional group is a cation exchange electrolyte having proton conductivity. An example of a fluorine-based cation exchange electrolyte is at least one selected from the group consisting of Nafion (registered trademark, manufactured by DuPont), Flemion (registered trademark, manufactured by Asahi Glass Co., Ltd.), Aciplex (registered trademark, manufactured by Asahi Kasei Corporation), and Gore-Select (registered trademark, manufactured by Gore Japan LLC). An example of a hydrocarbon-based cation exchange electrolyte is at least one selected from the group consisting of sulfonated polyether ketone, sulfonated polyether sulfone, sulfonated polyether ether sulfone, sulfonated polysulfide, and sulfonated polyphenylene.

[0098] When the outer coating layer 14C contains a polymer having a Lewis acidic functional group in its molecular structure, a polymer electrolyte having hydroxide ion conductivity is adsorbed to the polymer having Lewis acidic functional groups (outer coating layer), thereby improving the mechanical properties of the electrode catalyst layer, such as suppressing the occurrence of cracks in the electrode catalyst layer, thereby improving durability. In addition to the improved mechanical properties, the adsorption of the hydroxide ion-conductive polymer electrolyte onto the coated fiber 14 forms a conduction path for hydroxide ions, resulting in high electrolysis performance. In other words, the hydroxide ion-conductive polymer electrolyte can be more strongly adsorbed to the coated fiber 14 via the outer coating layer 14C containing a polymer having a Lewis acidic functional group than by directly adsorbing the hydroxide ion-conductive polymer electrolyte onto the fiber core 14A.

[0099] On the other hand, when the outer coating layer 14C containing the polymer having a Lewis acidic functional group is not used, the mechanical properties of the electrode catalyst layer are insufficient, it is difficult to suppress the occurrence of cracks, and it is presumed that durability cannot be improved. Furthermore, since the polymer electrolyte having hydroxide ion conductivity is dispersed, the formation of a conduction path for hydroxide ions is inhibited, and it is presumed that electrolysis performance cannot be improved.

[0100] The outer coating layer 14C preferably contains a polymer containing a Lewis acidic functional group as a main component. The main component means that the polymer accounts for 50% by mass or more. The mass ratio of the polymer containing a Lewis acidic functional group in the outer coating layer 14C may be 70%, 80%, or 90% by mass.

[0101] There is no particular limitation on the thickness of the outer coating layer 14C, but it may be, for example, about 20 to 100 nm.

[0102] (Intermediate coating layer 14B) The intermediate coating layer 14B contains a polymer having a Lewis basic functional group in its molecular structure. A Lewis basic functional group is a functional group capable of donating an electron pair. Examples of Lewis basic functional groups are imide structures and / or azole structures. Examples of polymers having an imide structure are polyimides such as aromatic polyimides. An example of an azole structure is a benzazole structure, and examples of benzazole structures are benzimidazole structures, benzoxazole structures, and benzothiazole structures. Examples of these polymers include polybenzimidazole, polybenzoxazole, and polyenzothiazole.

[0103] Polybenzimidazole is a polymer suitable for coating carbon fibers because its molecular structure contains a basic moiety that interacts with the polymer (outer coating layer) containing Lewis acidic functional groups contained in the outer coating layer 14C and a benzene ring moiety that interacts with the carbon of the fiber core 14A. Specifically, by providing the intermediate coating layer 14B between the carbon fiber core 14A and the outer coating layer 14C, adhesion between the carbon fiber core 14A and the intermediate coating layer 14B is improved. Furthermore, by providing the outer coating layer 14C containing a polymer containing Lewis acidic functional groups on the intermediate coating layer 14B containing a polymer with Lewis basic functional groups, adhesion between the intermediate coating layer 14B and the outer coating layer 14C is also improved. As a result, a polymer electrolyte with hydroxide ion conductivity can be strongly adsorbed onto the coated fiber 14.

[0104] The intermediate coating layer 14B preferably contains a polymer containing a Lewis basic functional group as a main component. The main component means that the polymer accounts for 50% by mass or more. The mass ratio of the polymer containing a Lewis basic functional group in the intermediate coating layer 14B may be 70% by mass, 80% by mass, or 90% by mass.

[0105] The intermediate coating layer 14B preferably contains polybenzimidazole as its main component. The term "main component" means that the polybenzimidazole accounts for 50% by mass or more. The mass percentage of polybenzimidazole may be 70%, 80%, or 90% by mass.

[0106] The polybenzimidazole is not particularly limited as long as it contains a benzimidazole structure in the repeating unit.

[0107] There is no particular limitation on the thickness of the intermediate coating layer 14B, but it may be, for example, about 1 to 5 nm.

[0108] (Mechanism of Action) The inventors of the present application have confirmed that the electrode catalyst layer having the above-described configuration has high mechanical properties and also exhibits high electrolysis performance. The detailed mechanism is speculated as follows, but the present invention is not limited to the mechanism described below.

[0109] In the coated fiber 14, the polymer electrolyte having hydroxide ion conductivity is adsorbed to the polymer having Lewis acid functional groups in the outer coating layer 14C, thereby improving the mechanical properties of the electrode catalyst layer and improving durability, such as by suppressing the occurrence of cracks in the electrode catalyst layer. In addition to the improved mechanical properties, the side polymer electrolyte having hydroxide ion conductivity is adsorbed onto the coated fiber 14, forming a conduction path for hydroxide ions, thereby achieving high electrolysis performance.

[0110] On the other hand, if a polymer having a Lewis acid functional group is not used in the outer coating layer 14C, the mechanical properties of the electrode catalyst layer will be insufficient, making it difficult to suppress the occurrence of cracks and making it impossible to improve durability.Furthermore, since a polymer electrolyte having hydroxide ion conductivity is dispersed, the formation of a conduction path for hydroxide ions will be inhibited and electrolysis performance will not be improved.

[0111] In the coated fiber 14, by having the intermediate coating layer 14B between the fiber core 14A and the outer coating layer 14C, the polymer containing a Lewis acidic functional group contained in the outer coating layer 14C is adsorbed to the polymer containing a Lewis basic functional group in the intermediate coating layer 14B, thereby improving the adhesion of the outer coating layer 14C and further improving durability. In addition, by using a polymer containing polybenzimidazole as the main component for the intermediate coating layer 14B, the adhesion between the carbon fiber of the fiber core 14A and the outer coating layer 14C is improved, thereby further improving durability.

[0112] Furthermore, if the fiber core 14A of the coated fiber 14 is vapor-grown carbon fiber (VGCF), it is likely that the carbon surfaces will have an annual ring structure in which they are stacked concentrically, which is likely to increase the affinity with the intermediate coating layer 14B.

[0113] The average fiber diameter of the coated fibers 14 is not particularly limited, but is preferably 50 nm to 1 μm, and more preferably 0.1 to 0.4 μm. In this case, the occurrence of cracks in the electrode catalyst layer is more likely to be suppressed. It is also possible to improve the adhesion between the polymer electrolyte membrane and the electrode catalyst layer. This can suppress the occurrence of voids due to peeling between the polymer electrolyte membrane and the electrode catalyst layer, and further suppress the increase in resistance of the membrane electrode assembly caused by these voids. It is estimated that if the average fiber diameter of the coated fibers is less than 50 nm, it may be difficult to improve the mechanical properties. It is also estimated that if the average fiber diameter of the coated fibers exceeds 1 μm, they may not be able to be dispersed as an ink.

[0114] The average fiber diameter refers to the average diameter measured for the cross section of the exposed coated fibers when the cross section of the electrode catalyst layer is observed using a scanning electron microscope (SEM). When the coated fibers are cut obliquely to their major axis, an elliptical cross section is obtained. In this case, the diameter refers to the diameter of a perfect circle fitted along the minor axis of the ellipse. Furthermore, when the cross section of the electrode catalyst layer is observed using an SEM, the surface of the coated fibers may be exposed rather than the cross section of the coated fibers. In this case, the diameter refers to the width of the fibers perpendicular to the major axis of the exposed coated fibers. The average fiber diameter of the coated fibers refers to the arithmetic mean value of fiber diameters obtained by similar measurements at at least 20 observation points.

[0115] As a method for exposing the cross section of the electrode catalyst layer, known methods such as ion milling and ultramicrotome can be used.

[0116] The average fiber length of the coated fibers is not particularly limited, but is preferably 500 nm or more, more preferably 1 μm or more. In this case, the coated fibers become entangled to form pores of appropriate size in the electrode catalyst layer, and the mechanical properties of the electrode catalyst layer can be improved. However, the average fiber length of the coated fibers is preferably 100 μm or less, more preferably 40 μm or less.

[0117] The average fiber length of the coated fibers refers to the arithmetic mean value of the fiber lengths obtained by measuring the lengths of at least 10 coated fibers. The average fiber length of the coated fibers in the electrode catalyst layer can be determined by measuring the particle size distribution using a solution in which the electrode catalyst layer is dissolved in a solvent. Specifically, the correlation between the average fiber length determined using an electron microscope and the peak position in the particle size distribution measurement is determined in advance, and the average fiber length of the coated fibers in the electrode catalyst layer is determined based on this correlation and the peak position determined by the particle size distribution measurement.

[0118] The composition of the cathode-side electrode catalyst layer 2 is not particularly limited, but the mass of the catalyst particles can be 1, the mass of the polymer electrolyte (solid content) can be 0.1 to 0.4, and the mass of the coated fiber can be 0.025 to 0.25.

[0119] (Anode-side electrode catalyst layer 3) As shown in Fig. 2, the anode-side electrode catalyst layer 3 includes catalyst particles 22 and a polymer electrolyte 23. Including the coated fibers 14 in the anode-side electrode catalyst layer 3, like the cathode-side electrode catalyst layer 2, improves the mechanical properties of the electrode catalyst layer and improves durability. In addition to the improved mechanical properties, the polymer electrolyte having hydroxide ion conductivity is adsorbed onto the coated fibers 14, forming a conduction path for hydroxide ions and achieving high electrolysis performance.

[0120] (Catalyst Particles) The catalyst particles 22 are particulate. When improved activity of the catalyst particles is required, the average particle size of the catalyst particles is preferably 20 nm or less, and more preferably 5 nm or less. When stabilization of the activity of the catalyst particles is required, the average particle size of the catalyst particles is preferably 0.5 nm or more, and more preferably 1 nm or more.

[0121] The catalyst particles in the anode-side electrode catalyst layer are catalysts for carrying out oxidation reactions. The constituent materials of the catalyst particles can be metals included in the platinum group, metals other than the platinum group, or alloys, oxides, double oxides, and carbides thereof. Among these, ruthenium, rhodium, palladium, iridium, platinum, and alloys containing at least one of these metals are preferred due to their high catalytic activity. The catalyst particles may be composed of only one of the above-mentioned examples, or a combination of two or more of them.

[0122] The catalyst particles of the anode-side electrode catalyst layer may be supported on a carrier 25. The carrier is a particle that is conductive and is not eroded in an oxidizing atmosphere. An example of the carrier is an oxide particle containing titanium, tin, or zirconium. When an expansion of the electron conduction path is required, the particle size of the carrier is preferably 10 nm or more. When a reduction in the resistance value of the electrode catalyst layer or an increase in the amount of catalyst particles supported is required, the particle size of the carrier is preferably 1000 nm or less, and more preferably 100 nm or less.

[0123] (Anode-Side Polymer Electrolyte) As the polymer electrolyte 23, a polymer electrolyte 23 having hydroxide ion conductivity similar to that of the polymer electrolyte in the cathode-side electrode catalyst layer can be used.

[0124] (Polymer electrolyte membrane 1) An example of the polymer electrolyte membrane 1 is a polymer electrolyte membrane having hydroxide ion conductivity, a so-called anion exchange resin membrane. The polymer electrolyte membrane is not particularly limited as long as it conducts hydroxide ions. For example, there are fluorine-based anion exchange electrolyte membranes and hydrocarbon-based anion exchange electrolyte membranes. Examples of fluorine-based electrolyte membranes include perfluorocarbon-based electrolyte membranes, and examples of hydrocarbon-based electrolyte membranes include styrene-based electrolyte membranes and acrylic-based electrolyte membranes.

[0125] When it is required to improve the adhesion between the electrode catalyst layer and the polymer electrolyte membrane, if the constituent material of the polymer electrolyte of the electrode catalyst layer is a fluorine-based polymer electrolyte, it is preferable that the constituent material of the polymer electrolyte membrane is also a fluorine-based polymer electrolyte. Furthermore, if the constituent material of the polymer electrolyte of the electrode catalyst layer is a hydrocarbon-based polymer electrolyte, it is preferable that the constituent material of the polymer electrolyte membrane is also a hydrocarbon-based polymer electrolyte. Furthermore, it is preferable that the constituent material of the polymer electrolyte membrane is the same as the constituent material of the polymer electrolyte of the electrode catalyst layer.

[0126] [Method for Manufacturing Membrane Electrode Assembly] Next, an example of a method for manufacturing the membrane electrode assembly having the above-described configuration will be described.

[0127] The membrane electrode assembly is produced by a method including the following first to third steps.

[0128] The first step is to form a polymer (intermediate coating layer) containing a Lewis basic functional group such as polybenzimidazole on the surface of vapor grown carbon fiber (VGCF) or the like.

[0129] The second step is a step of forming a coated fiber by coating the surface of the conductive fiber core coated with the intermediate coating layer obtained in the first step with a polymer (outer coating layer) containing a Lewis acid functional group.

[0130] The third step is a step of producing a cathode-side catalyst ink containing catalyst particles, a polymer electrolyte, the coated fiber obtained in the second step, and a solvent, and a step of producing an anode-side catalyst ink containing catalyst particles, a polymer electrolyte, and a solvent.

[0131] The fourth step is a step of applying the anode-side catalyst ink and cathode-side catalyst ink obtained in the third step onto a polymer electrolyte membrane and drying the solvent, thereby forming an anode-side electrode catalyst layer and a cathode-side electrode catalyst layer on both sides of the polymer electrolyte membrane.

[0132] [Detailed Description] (Step 1) A polymer containing a Lewis basic functional group, such as polybenzimidazole, is dissolved or dispersed in a solvent to prepare a polymer dispersion / solution. An example of the solvent is dimethylacetamide. Fiber cores are added to this polymer dispersion / solution, and ultrasonic dispersion treatment is performed as needed. The solid content is then recovered by filtration and dried, forming an intermediate coating layer on the surface of the fiber core.

[0133] (Step 2) A polymer containing a Lewis basic functional group, such as a cation exchange electrolyte, is dissolved or dispersed in a solvent to prepare a polymer dispersion / solution. Examples of solvents include alcohols. The conductive fiber core coated with the intermediate coating layer obtained in Step 1 is added to this polymer dispersion / solution, and ultrasonic dispersion treatment is performed as necessary. The solid content is then recovered by filtration and dried, forming a peripheral coating layer on the surface of the intermediate coating layer.

[0134] (Step 3) The solvent constituting the catalyst ink does not corrode the catalyst particles, polymer electrolyte, and coated fibers, and dissolves the polymer electrolyte or disperses it as a fine gel. An example of the solvent constituting the catalyst ink is at least one selected from the group consisting of alcohols, ketone-based solvents, ether-based solvents, and polar solvents. An example of the alcohol is at least one selected from the group consisting of methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, isobutyl alcohol, tert-butyl alcohol, and pentanol. An example of the ketone-based solvent is at least one selected from the group consisting of acetone, methyl ethyl ketone, pentanone, methyl isobutyl ketone, heptanone, cyclohexanone, methylcyclohexanone, acetonyl acetone, and diisobutyl ketone. An example of the ether-based solvent is at least one selected from the group consisting of tetrahydrofuran, dioxane, diethylene glycol dimethyl ether, anisole, methoxytoluene, and dibutyl ether. An example of the polar solvent is at least one selected from the group consisting of dimethylformamide, dimethylacetamide, N-methylpyrrolidone, ethylene glycol, diethylene glycol, diacetone alcohol, and 1-methoxy-2-propanol. The solvent constituting the catalyst ink may contain water, which has a high affinity for the polymer electrolyte.

[0135] When improved dispersibility of catalyst particles is required, the catalyst ink preferably contains a dispersant. Examples of dispersants include anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants. When improved dispersibility of the catalyst ink is required, a dispersion treatment is preferably performed in the production of the catalyst ink. Examples of dispersion treatments include stirring with a ball mill and a roll mill, stirring with a shear mill, stirring with a wet mill, stirring by applying ultrasonic waves, and stirring with a homogenizer.

[0136] When suppression of cracking on the surface of the electrode catalyst layer is required, the solid content of the catalyst ink is preferably 50% by mass or less.When an improvement in the film formation rate of the electrode catalyst layer is required, the solid content of the catalyst ink is preferably 1% by mass or more.

[0137] (Fourth Step) Examples of methods for applying the catalyst ink onto a substrate include a doctor blade method, a dipping method, a screen printing method, or a roll coating method. The substrate to which the catalyst ink is applied is a transfer sheet. Examples of materials constituting the transfer sheet include a fluorine-based resin or an organic polymer compound other than a fluorine-based resin. Examples of fluorine-based resins include ethylene tetrafluoroethylene copolymer (ETFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroperfluoroalkylvinyl ether copolymer (PFA), or polytetrafluoroethylene (PTFE). Examples of organic polymer compounds include polyimide, polyethylene terephthalate, polyamide, polysulfone, polyethersulfone, polyphenylene sulfide, polyether ether ketone, polyetherimide, polyarylate, and polyethylene naphthalate.

[0138] In the above embodiment, the coated fiber is provided on the electrode catalyst layer on the cathode side, but it may also be provided on the electrode catalyst layer on the anode side.

[0139] Hereinafter, the electrode catalyst layer and membrane electrode assembly for a water electrolysis apparatus according to this embodiment will be described with reference to specific examples and comparative examples, but this embodiment is not limited to the following examples and comparative examples.

[0140] <Effects and Others> According to this embodiment, it is possible to manufacture a membrane electrode assembly for a water electrolysis system having an electrode catalyst layer with high mechanical properties and excellent electrolysis performance and durability, without using complicated processes.

[0141] Example B1 [Production of Coated Fiber] Polybenzimidazole of the following formula was dissolved in dimethylacetamide to prepare a polybenzimidazole dispersion. Next, carbon fibers (VGCF-H (registered trademark), vapor-grown carbon fibers manufactured by Showa Denko K.K.) with an average fiber diameter of 0.15 μm were added to this polybenzimidazole dispersion, and ultrasonic dispersion treatment was performed. Subsequently, filtration and drying were performed to obtain polybenzimidazole-coated carbon fibers. The thickness of the polybenzimidazole coating layer was as thin as a few nanometers, and the average fiber diameter of the obtained polybenzimidazole-coated carbon fibers was substantially the same as that of the core fibers.

[0142] A fluorine-based polymer electrolyte (Nafion (registered trademark) dispersion) was dissolved as a cation exchange electrolyte in a mixed solvent of ultrapure water and 1-propanol to prepare a fluorine-based polymer electrolyte dispersion. The volume ratio of ultrapure water to 1-propanol was 1:1. The solid content in the dispersion was adjusted to 1 mass %. Next, polybenzimidazole-coated carbon fibers were added to this fluorine-based polymer electrolyte dispersion, and an ultrasonic dispersion treatment was performed. After that, filtration and drying were performed to obtain coated fibers having carbon fibers as a conductive fiber core, polybenzimidazole as an intermediate coating layer, and a fluorine-based polymer electrolyte as an outer coating layer. The average fiber diameter of the obtained coated fibers was approximately 0.25 μm.

[0143] [Production of anode-side catalyst ink] The catalyst particles and polymer electrolyte shown below were mixed in a solvent and dispersed for 30 minutes using a planetary ball mill to produce a catalyst ink. A mixed solvent of ultrapure water and 1-propanol was used as the solvent for the catalyst ink. The volume ratio of ultrapure water to 1-propanol was 1:1. The catalyst ink was adjusted so that the solid content in the catalyst ink was 10% by mass. - Catalyst particles: iridium oxide - Polymer electrolyte: hydrocarbon-based anion exchange electrolyte - Blending ratio: The mass of the catalyst particles in the catalyst ink was 1, and the mass of the polymer electrolyte (solids) was 0.2.

[0144] [Production of Cathode-Side Catalyst Ink] The catalyst particles, polymer electrolyte, and coated fibers shown below were mixed in a solvent and dispersed for 30 minutes using a planetary ball mill to produce a catalyst ink. The solvent used for the catalyst ink was a mixed solvent of ultrapure water and 1-propanol. The volume ratio of ultrapure water to 1-propanol was 1:1. The catalyst ink was adjusted so that the solid content in the catalyst ink was 10% by mass. Catalyst particles: Pt-supported carbon particles Ionomer: hydrocarbon-based anion exchange electrolyte Blending ratio: The catalyst ink had a catalyst particle mass of 1, a polymer electrolyte (solids) mass of 0.3, and a coated fiber mass of 0.05.

[0145] [Fabrication of Membrane Electrode Assembly] The prepared cathode catalyst ink was applied to one side of a polymer electrolyte membrane (hydrocarbon-based anion exchange electrolyte membrane) using a die coater to form a rectangular coating film measuring 50 mm long x 50 mm wide. The cathode catalyst ink was applied in an amount that resulted in a catalyst content of 0.5 mg / cm². A drying process was then performed using an oven at 60°C to volatilize the dispersion medium contained in the coating film, thereby forming a cathode electrode catalyst layer. Next, the prepared anode catalyst ink was applied to the side of the polymer electrolyte membrane opposite the side on which the cathode electrode catalyst layer was formed, thereby forming a rectangular coating film measuring 50 mm long x 50 mm wide. The anode catalyst ink was applied in an amount that resulted in a catalyst content of 0.5 mg / cm². The coating was then dried using an oven at 60°C to volatilize the dispersion medium contained in the coating film, thereby forming an anode electrode catalyst layer, thereby obtaining a membrane electrode assembly. Both electrode catalyst layers of Example B1 were free from cracks and did not peel off from the polymer electrolyte membrane.

[0146] Example B2 A membrane electrode assembly of Example B2 was obtained in the same manner as in Example B1, except that carbon fibers having an average fiber diameter of 0.8 μm were used as the fiber cores in the coated fibers. Both electrode catalyst layers of Example B2 were free from cracks and did not peel off from the polymer electrolyte membrane.

[0147] Comparative Example B1 A membrane electrode assembly of Comparative Example B1 was obtained in the same manner as in Example B1, except that uncoated carbon fibers (VGCF-H (registered trademark), vapor-grown carbon fibers manufactured by Showa Denko K.K.) having an average fiber diameter of 0.15 μm were used instead of the coated fibers.

[0148] In Comparative Example B1, no cracks were observed during the formation of the cathode-side electrode catalyst layer, and no peeling from the polymer electrolyte membrane occurred. However, cracks occurred in the cathode-side electrode catalyst layer during the formation of the anode-side electrode catalyst layer, and partial peeling from the polymer electrolyte membrane was observed.

[0149] Comparative Example B2: A membrane electrode assembly of Comparative Example B2 was obtained using the same procedure as in Example B1, except that no coated fibers were used. Significant cracking occurred during the formation of the cathode-side electrode catalyst layer of Comparative Example B2, and significant peeling from the polymer electrolyte membrane was observed. Therefore, it was not possible to apply the anode-side catalyst ink.

[0150] When the membrane electrode assemblies obtained in Examples B1 and B2 and Comparative Examples B1 and B2 were immersed in water, the electrode catalyst layers of both Examples B1 and B2 did not peel off from the polymer electrolyte membrane, but the cathode-side electrode catalyst layer of Comparative Example B1 peeled off from the polymer electrolyte membrane. Furthermore, when the water electrolysis performance was evaluated using each membrane electrode assembly, the membrane electrode assemblies obtained in Examples B1 and B2 exhibited good electrolysis performance, but the membrane electrode assembly obtained in Comparative Example B1 exhibited a significant decrease in electrolysis performance after repeated electrolysis. The electrolysis performance results for the membrane electrode assemblies prepared in the Examples and Comparative Examples confirmed that the membrane electrode assemblies prepared in the Examples had sufficient adhesion strength between the cathode-side electrode catalyst layer and the electrolyte membrane, and good electrolysis performance was obtained.

[0151] <Water Electrolysis Apparatus> An embodiment of a water electrolysis apparatus according to the present disclosure will be described with reference to Fig. 4. Fig. 4 is a cross-sectional view showing an embodiment of a water electrolysis apparatus 300 according to the present disclosure.

[0152] As shown in FIG. 4 , the water electrolysis apparatus 300 of this embodiment includes a membrane electrode assembly 11, an anode-side current collector 310 and a cathode-side current collector 320 disposed so as to sandwich the membrane electrode assembly 11 therebetween, and a DC power supply (not shown) electrically connected to the anode-side current collector 310 and the cathode-side current collector 320.

[0153] The anode-side current collector 310 is connected to a DC power supply to function as an anode, and the anode-side current collector 310 is joined to the electrode catalyst layer 20 of the membrane electrode assembly 200. The cathode-side current collector 320 is connected to a DC power supply to function as a cathode, and the cathode-side current collector 320 is joined to the electrode catalyst layer 30 of the membrane electrode assembly 200.

[0154] The current collector may be any conductive material. Specific examples include carbon paper, carbon nonwoven fabric, and oxide and metal plates. Examples of metal plates include titanium sintered bodies. The carbon paper may be water-repellent, and the oxide and metal plates may be plated with a precious metal. The current collector may be porous or may have flow paths for supplying or discharging gases or liquids. The current collector may function as a separator that retains liquids and gases supplied to the cathode and anode sides or generated and discharged.

[0155] In the case of a water electrolysis device, when water and voltage are supplied, oxygen and protons are generated from water at the electrode catalyst layer on the anode side in the case of a proton exchange membrane type, and the generated protons are converted to hydrogen at the electrode catalyst layer on the cathode side, while in the case of an anion exchange membrane type, hydrogen and hydroxide ions are generated from water at the electrode catalyst layer on the cathode side, and the generated hydroxide ions are converted to oxygen and water at the electrode catalyst layer on the anode side. Ultrapure water or other water is used as the water.

[0156] Although the embodiments of the present invention have been described in detail above, in reality, the present invention is not limited to the above-described embodiments, and even if modifications are made within the scope of the gist of the present invention, they are included in the present invention.

[0157] REFERENCE SIGNS LIST 1... polymer electrolyte membrane, 2... cathode side electrode catalyst layer, 3... anode side electrode catalyst layer, 11... membrane electrode assembly, 14α... ionomer-adsorbing carbon fiber, 14... coated fiber

Claims

1. An electrocatalyst layer comprising catalyst particles, an ionomer, and an ionomer-adsorbing carbon fiber capable of adsorbing the ionomer.

2. The electrode catalyst layer according to claim 1, wherein the ionomer-adsorbing carbon fiber has the ionomer adsorbed thereon, and the amount of the ionomer adsorbed is 10 mg or more per gram of the ionomer-adsorbing carbon fiber.

3. The electrode catalyst layer according to claim 1 or 2, wherein the average fiber diameter of the ionomer-adsorbing carbon fibers is within the range of 50 nm or more and 1 μm or less.

4. The electrode catalyst layer according to claim 1 or 2, wherein the ionomer-adsorbing carbon fiber is a hydrophilically treated carbon fiber.

5. The electrode catalyst layer according to claim 1 or 2, wherein the ionomer-adsorbing carbon fiber is a vapor-grown carbon fiber (VGCF) that has been hydrophilically treated.

6. The electrode catalyst layer according to claim 1 or 2, which is for a water electrolysis device.

7. The electrode catalyst layer according to claim 6, which is a cathode-side electrode catalyst layer.

8. A membrane electrode assembly comprising a polymer electrolyte membrane, and an anode-side electrode catalyst layer and a cathode-side electrode catalyst layer sandwiching the polymer electrolyte membrane, wherein at least one of the cathode-side electrode catalyst layer and the anode-side electrode catalyst layer is the electrode catalyst layer described in claim 1 or 2.

9. An electrode catalyst layer comprising catalyst particles, a polymer electrolyte having hydroxide ion conductivity, and a coated fiber, the coated fiber having a fiber core and a peripheral coating layer coating the peripheral surface of the fiber core, the peripheral coating layer containing a polymer having a Lewis acidic functional group.

10. The electrode catalyst layer according to claim 9, wherein the coated fiber has an intermediate coating layer between the fiber core and the outer coating layer, and the intermediate coating layer contains a polymer compound having a Lewis basic functional group.

11. The electrode catalyst layer according to claim 10, wherein the polymer compound of the intermediate coating layer has an azole structure.

12. The electrode catalyst layer according to claim 10, wherein the polymer compound of the intermediate coating layer is polybenzimidazole.

13. The electrode catalyst layer according to claim 9 or 10, wherein the fiber core is a conductive fiber.

14. The electrode catalyst layer according to claim 13, wherein the conductive fibers are carbon fibers.

15. The electrocatalyst layer of claim 14, wherein the carbon fibers are vapor grown carbon fibers (VGCF).

16. The electrode catalyst layer according to claim 9 or 10, wherein the average fiber diameter of the coated fibers is within the range of 50 nm to 1 μm.

17. The electrode catalyst layer according to claim 9 or 10, which is for an anion exchange membrane water electrolysis cell.

18. The electrode catalyst layer according to claim 17, which is a cathode-side electrode catalyst layer.

19. A membrane electrode assembly comprising a polymer electrolyte membrane, and an anode side electrode catalyst layer and a cathode side electrode catalyst layer sandwiching the polymer electrolyte membrane, wherein the cathode side electrode catalyst layer is an electrode catalyst layer according to claim 9 or 10.

Citation Information

Patent Citations

  • Paste for forming electrode catalyst layer, manufacturing method, film-electrode catalyst layer conjugant, gas diffusion electrode, solid polymer fuel cell, and manufacturing method of solid polymer water electrolysis cell

    JP2019083085A

  • Paste for forming electrode catalyst layer and method for manufacturing same, and methods for manufacturing membrane-electrode catalyst layer assembly, gas diffusion electrode, solid polymer fuel cell and solid polymer water electrolysis cell

    WO2017159820A1

  • A fuel cell's electrode and its a durability improvingmethod

    KR1020070112978A

  • Gas Diffusion Electrodes and Methods for Fabricating and Testing Same

    US20150376803A1

  • Membrane-electrode assembly for fuel cells and solid polymer fuel cell

    WO2020075777A1

Cited By

  • Electrolysis cell and electrolysis device

    WO2025154357A1