Pressure-sensitive adhesive sheet and display body

The pressure-sensitive adhesive sheet addresses the issue of needle-like cracks in display modules by maintaining a stable gel fraction and molecular structure, ensuring enhanced weather resistance and image quality under UV exposure.

WO2024202754A1PCT designated stage expired Publication Date: 2024-10-03LINTEC CORP

Patent Information

Application Number
PCT/JP2024/006471
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-02-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

The existing adhesive layers used in display modules, especially when exposed to high-intensity ultraviolet rays, tend to develop needle-like cracks, leading to deteriorated image quality and reduced weather resistance due to changes in the crosslinking structure.

Method used

A pressure-sensitive adhesive sheet with an adhesive layer that maintains a gel fraction of 30% to 95% and a gel fraction change rate of 117% or less after ultraviolet irradiation, along with specific molecular weight and storage modulus ranges, suppresses the formation of needle-like cracks and enhances weather resistance.

Benefits of technology

The adhesive sheet effectively prevents the occurrence of needle-like cracks and ensures excellent weather resistance by maintaining the adhesive's structural integrity and cohesive force even after prolonged exposure to high-intensity ultraviolet rays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024006471_03102024_PF_FP_ABST
    Figure JP2024006471_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A pressure-sensitive adhesive sheet 1 has a pressure-sensitive adhesive agent layer 11 for pasting together two display body constituting members. When G1 represents the gel fraction of a pressure-sensitive adhesive agent constituting the pressure-sensitive adhesive agent layer 11 after being pasted and G2 represents the gel fraction of the pressure-sensitive adhesive agent constituting the pressure-sensitive adhesive agent layer 11 after ultraviolet rays having an illumination intensity of 100 mW / cm2 are applied for 120 hours on the pressure-sensitive adhesive agent layer 11 after being pasted, G1 equals 30-95%, and the gel fraction change ratio which is the ratio of G2 with respect to G1 is 117% or less. The pressure-sensitive adhesive sheet 1 can suppress occurrence of needle-like cracks and has excellent weather resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Adhesive sheets and displays

[0001] The present invention relates to an adhesive sheet for bonding two display component members together, and to an indicator obtained by using an adhesive layer of the adhesive sheet.

[0002] BACKGROUND ART In recent years, various mobile electronic devices such as mobile phones, smartphones, and tablet terminals are equipped with displays that use display modules having liquid crystal elements, light-emitting diodes (LED elements), organic electroluminescence (organic EL) elements, etc.

[0003] In such displays, a protective panel is usually provided on the front side of the display module. As electronic devices become thinner and lighter, the protective panel is increasingly being replaced by a plastic plate such as an acrylic plate or a polycarbonate plate, rather than the conventional glass plate.

[0004] Here, a gap is provided between the protective panel and the display module so that even when the protective panel is deformed by an external force, the deformed protective panel will not collide with the display module.

[0005] However, when such a gap, i.e., an air layer, is present, there is a problem that the difference in refractive index between the protective panel and the air layer, and the difference in refractive index between the air layer and the display module, results in a large light reflection loss, which reduces the image quality of the display.

[0006] Therefore, it has been proposed to improve the image quality of a display by filling the gap between the protective panel and the display module with an adhesive layer. For example, Patent Document 1 discloses an adhesive layer having a shear storage modulus (G') of 1.0 x 10 at 25°C and 1 Hz, which is used to fill the gap between the protective panel and the display module. 5 The document discloses a pressure-sensitive adhesive layer having a viscosity of 100 Pa or less and a gel fraction of 40% or more.

[0007] JP 2010-97070 A

[0008] However, when a display obtained using the above-described pressure-sensitive adhesive layer is irradiated with high-intensity ultraviolet light for a long period of time, needle-like cracks may occur in the pressure-sensitive adhesive layer. In particular, such a problem is likely to occur when an accelerated weather resistance test is performed in which high-intensity ultraviolet light is irradiated for a long period of time.

[0009] The present invention has been made in view of the above circumstances, and has an object to provide a pressure-sensitive adhesive sheet and a display that can suppress the occurrence of needle-like cracks and have excellent weather resistance.

[0010] In order to achieve the above object, first, the present invention provides a pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer for bonding two display component members to each other, wherein the gel fraction of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer after bonding is defined as G1, and the illuminance of the pressure-sensitive adhesive layer after bonding is 100 mW / cm. 2 The present invention provides a pressure-sensitive adhesive sheet characterized in that, when the gel fraction of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer after 120 hours of irradiation with ultraviolet light of 1000 kJ / cm² is defined as G2, G1 is 30% or more and 95% or less, and the gel fraction change rate, which is the ratio of G2 to G1, is 117% or less (Invention 1).

[0011] In the pressure-sensitive adhesive of the pressure-sensitive adhesive sheet according to the above invention (Invention 1), even when exposed to high-intensity ultraviolet light for a long period of time (e.g., 20 hours, 40 hours, etc.), structural changes that could become the starting point for needle-like cracks (e.g., destruction of crosslinking points) are suppressed. As a result, the pressure-sensitive adhesive sheet can suppress the occurrence of needle-like cracks and has excellent weather resistance.

[0012] In the above invention (Invention 1), it is preferable that the average peak molecular weight of the sol component of the adhesive constituting the adhesive layer after lamination is 10,000 or more and 250,000 or less (Invention 2).

[0013] In the above inventions (Inventions 1 and 2), the illuminance of the pressure-sensitive adhesive layer after lamination is 100 mW / cm 2 It is preferable that the average peak molecular weight of the sol component of the adhesive constituting the adhesive layer after 120 hours of irradiation with ultraviolet light of 10,000 or more and 200,000 or less (Invention 3).

[0014] In the above inventions (Inventions 1 to 3), it is preferable that the storage modulus G' at 23° C. of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer after lamination is 0.01 MPa or more and 2 MPa or less (Invention 4).

[0015] In the above inventions (Inventions 1 to 4), the illuminance of the pressure-sensitive adhesive layer after lamination is 100 mW / cm 2 It is preferable that the storage modulus G' of the adhesive constituting the adhesive layer at 23°C after irradiation with ultraviolet light of 1000 kJ / cm2 for 120 hours is 0.01 MPa or more and 2 MPa or less (Invention 5).

[0016] In the above inventions (Inventions 1 to 5), it is preferable that the storage modulus G' at -15°C of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer after lamination is 0.01 MPa or more and 100 MPa or less (Invention 6).

[0017] In the above inventions (Inventions 1 to 6), the illuminance of the pressure-sensitive adhesive layer after lamination is 100 mW / cm 2 It is preferable that the storage modulus G' of the adhesive constituting the adhesive layer at -15°C after irradiation with ultraviolet light of 120 hours is 0.1 MPa or more and 1000 MPa or less (Invention 7).

[0018] In the above inventions (Inventions 1 to 7), it is preferable that the storage modulus G' at 100° C. of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer after lamination is 0.0001 MPa or more and 1 MPa or less (Invention 8).

[0019] In the above inventions (Inventions 1 to 8), the illuminance of the pressure-sensitive adhesive layer after lamination is 100 mW / cm 2 It is preferable that the storage modulus G' of the adhesive constituting the adhesive layer at 100°C after irradiation with ultraviolet light of 100°C for 120 hours is 0.0001 MPa or more and 1 MPa or less (Invention 9).

[0020] In the above inventions (Inventions 1 to 9), the peak temperature of the loss tangent tan δ of the adhesive constituting the adhesive layer after lamination is preferably −30° C. or higher and 30° C. or lower (Invention 10).

[0021] In the above inventions (Inventions 1 to 10), the illuminance of the pressure-sensitive adhesive layer after lamination is 100 mW / cm 2It is preferable that the peak temperature of the loss tangent tan δ of the adhesive constituting the adhesive layer after 120 hours of irradiation with ultraviolet light of 1000 kJ / cm 2 or less is −30° C. or more and 30° C. or less (Invention 11).

[0022] In the above inventions (Inventions 1 to 11), it is preferable that the adhesive constituting the adhesive layer is an active energy ray-curable adhesive, and the adhesive layer after lamination is an active energy ray-cured adhesive layer (Invention 12).

[0023] In the above invention (Invention 12), it is preferable that the gel fraction of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer before being cured with active energy rays is 20% or more and 85% or less (Invention 13).

[0024] In the above inventions (Inventions 1 to 13), the pressure-sensitive adhesive is preferably an acrylic pressure-sensitive adhesive (Invention 14).

[0025] In the above inventions (Inventions 1 to 14), it is preferable that the pressure-sensitive adhesive sheet comprises two release sheets, and the pressure-sensitive adhesive layer is sandwiched between the release sheets so as to contact the release surfaces of the two release sheets (Invention 15).

[0026] Secondly, the present invention provides a display comprising one display component, another display component, and an adhesive layer for bonding the one display component and the other display component to each other, wherein the adhesive layer is formed from the adhesive layer of the adhesive sheet (Inventions 1 to 15) (Invention 16).

[0027] In the above invention (Invention 16), both the one display member and the other display member may be hard plates (Invention 17).

[0028] The pressure-sensitive adhesive sheet and indicator according to the present invention can suppress the occurrence of needle-like cracks and have excellent weather resistance.

[0029] 1 is a cross-sectional view of a pressure-sensitive adhesive sheet according to one embodiment of the present invention;

[0030] Hereinafter, an embodiment of the present invention will be described. [Adhesive Sheet] The adhesive sheet according to this embodiment has an adhesive layer for bonding two display member components to each other. The specific configuration of the adhesive sheet and the display member components will be described later.

[0031] The gel fraction of the adhesive constituting the adhesive layer after lamination in the adhesive sheet according to this embodiment is defined as G1, and the illuminance of the adhesive layer after lamination is 100 mW / cm 2 When the gel fraction of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer after 120 hours of irradiation with ultraviolet light (hereinafter sometimes referred to as "S-UV irradiation") is defined as G2, it is preferable that G1 is 30% or more and 95% or less, and the gel fraction change rate ((G2 / G1)×100) (%), which is the ratio of G2 to G1, is 117% or less. The method for measuring the gel fraction in this specification is as shown in the test examples described later.

[0032] Here, in the present specification, "adhesive layer after lamination" refers to an adhesive layer in the same state as the adhesive layer of the adhesive sheet if the adhesive layer is not active energy ray-curable, or to an adhesive layer cured by active energy ray irradiation after lamination if the adhesive layer is active energy ray-curable. "Adhesive layer after active energy ray curing" refers to an adhesive layer that has been completely cured by active energy ray irradiation. Specifically, when the active energy ray-cured adhesive layer is further irradiated with active energy ray at the same dose (light amount) as when the active energy ray-cured adhesive layer was cured with the active energy ray, the increase in gel fraction of the adhesive layer is 10% or less, and particularly refers to an increase in gel fraction of 5% or less. Furthermore, in the present specification, "relative humidity α%" may be expressed as "α% RH" (RH; Relative humidity).

[0033] Generally, it is thought that prolonged irradiation with high-intensity ultraviolet light as described above causes changes in the crosslinking structure of the adhesive, resulting in needle-like cracks. In contrast, the adhesive of the present invention satisfies the above relational expression, thereby suppressing changes in the crosslinking structure of the adhesive even after prolonged irradiation with high-intensity ultraviolet light (e.g., 20 hours, 40 hours, etc.). As a result, structural changes that could serve as the starting point for needle-like cracks (e.g., destruction of crosslinking points) are suppressed. In this way, the adhesive sheet according to the present embodiment can suppress the occurrence of needle-like cracks and has excellent weather resistance.

[0034] From the viewpoint of suppressing needle-like cracks, the gel fraction change rate is more preferably 116% or less, and particularly preferably 115% or less. The lower limit of the gel fraction change rate is not particularly limited, but is preferably 100% or more, more preferably 102% or more, particularly preferably 104% or more, even more preferably 107% or more, and of these, preferably 109% or more.

[0035] As described above, G1 is preferably 30 to 95%, more preferably 40 to 92%, particularly preferably 50 to 90%, further preferably 55 to 88%, and of these, preferably 60 to 86%. This allows the PSA to exert a predetermined cohesive force, making it easier to obtain excellent weather resistance and to satisfy the above-mentioned gel fraction change rate.

[0036] G2 is preferably 40 to 99%, more preferably 50 to 98%, particularly preferably 60 to 97%, even more preferably 64 to 96%, and of these, preferably 67 to 95%. This allows the pressure-sensitive adhesive to exhibit a predetermined cohesive strength even after S-UV irradiation, making it easier to obtain excellent weather resistance.

[0037] When the pressure-sensitive adhesive layer in the pressure-sensitive adhesive sheet according to the present embodiment is active energy ray-curable, the gel fraction (G0) of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer before active energy ray curing is preferably 20 to 85%, more preferably 30 to 80%, particularly preferably 35 to 75%, and even more preferably 40 to 70%. This makes it easier for G1 to fall within the preferred range, and also makes it easier to obtain good adhesiveness when attached to an adherend.

[0038] In this embodiment, the average peak molecular weight of the sol component of the adhesive constituting the adhesive layer after lamination is preferably 10,000 to 250,000, more preferably 30,000 to 200,000, particularly preferably 50,000 to 150,000, even more preferably 60,000 to 100,000, and most preferably 63,000 to 80,000. This tends to ensure good adhesive strength after lamination of the display component. Note that the average peak molecular weight of the sol component in this specification is a value measured by gel permeation chromatography (GPC) in terms of standard polystyrene. Specific measurement methods are as shown in the test examples described below.

[0039] The average peak molecular weight of the sol component of the pressure-sensitive adhesive after S-UV irradiation of the pressure-sensitive adhesive layer after lamination (hereinafter simply referred to as "pressure-sensitive adhesive after S-UV irradiation") is preferably 10,000 to 200,000, more preferably 30,000 to 150,000, particularly preferably 50,000 to 100,000, and even more preferably 55,000 to 80,000. This makes it easier for the gel fraction change rate to fall within the preferred range.

[0040] The storage modulus G' at 23°C of the adhesive constituting the adhesive layer after lamination is preferably 0.01 to 2 MPa, more preferably 0.04 to 1.5 MPa, more preferably 0.08 to 1 MPa, particularly preferably 0.09 to 0.7 MPa, and even more preferably 0.1 to 0.5 MPa. This tends to result in good adhesive strength after lamination of the display component. The method for measuring the storage modulus G' in this specification is as shown in the test examples described below.

[0041] The storage modulus G' of the pressure-sensitive adhesive after S-UV irradiation at 23°C is preferably 0.01 to 2 MPa, more preferably 0.04 to 1.5 MPa, more preferably 0.08 to 1 MPa, particularly preferably 0.1 to 0.8 MPa, and even more preferably 0.2 to 0.6 MPa. This makes it easier for the gel fraction change rate to fall within the preferred range.

[0042] The storage modulus G' at -15°C of the adhesive constituting the adhesive layer after lamination is preferably 0.01 to 100 MPa, more preferably 0.1 to 80 MPa, more preferably 1 to 60 MPa, particularly preferably 3 to 50 MPa, even more preferably 6 to 40 MPa, and of these, preferably 8 to 30 MPa. This makes it easier to achieve good adhesive strength at low temperatures after lamination of the display component.

[0043] The storage modulus G' of the pressure-sensitive adhesive after S-UV irradiation at -15°C is preferably 0.1 to 1000 MPa, more preferably 1 to 100 MPa, more preferably 5 to 80 MPa, particularly preferably 10 to 60 MPa, even more preferably 15 to 50 MPa, and of these, preferably 20 to 45 MPa. This makes it easier for the gel fraction change rate to fall within the preferred range.

[0044] The storage modulus G' at 100°C of the adhesive constituting the adhesive layer after lamination is preferably 0.0001 to 1 MPa, more preferably 0.001 to 0.7 MPa, more preferably 0.004 to 0.4 MPa, particularly preferably 0.008 to 0.2 MPa, even more preferably 0.010 to 0.1 MPa, and of these, preferably 0.011 to 0.08 MPa. This makes it easier to achieve good adhesive strength at high temperatures after lamination of the display component.

[0045] The storage modulus G' of the pressure-sensitive adhesive after S-UV irradiation at 100°C is preferably 0.0001 to 1 MPa, more preferably 0.001 to 0.5 MPa, more preferably 0.005 to 0.2 MPa, particularly preferably 0.01 to 0.1 MPa, and even more preferably 0.015 to 0.09 MPa. This makes it easier for the gel fraction change rate to fall within the preferred range.

[0046] The peak temperature Tb of the loss tangent tanδ of the adhesive constituting the adhesive layer after lamination is preferably −30 to 30° C., more preferably −25 to 20° C., particularly preferably −20 to 10° C., even more preferably −16 to 0° C., and most preferably −12 to −8° C. This makes it easier to obtain good adhesive strength after lamination of the display component. The method for measuring the loss tangent tanδ is as shown in the test examples described below.

[0047] The peak temperature Ta of the loss tangent tanδ of the pressure-sensitive adhesive after S-UV irradiation is preferably −30 to 30° C., more preferably −20 to 20° C., particularly preferably −15 to 15° C., further preferably −10 to 10° C., and most preferably −7 to 2° C. This makes it easier for the gel fraction change rate to fall within the preferred range.

[0048] The value obtained by subtracting Tb from Ta (Ta - Tb) is preferably 0 to 30, more preferably 0.1 to 20, particularly preferably 1 to 15, and even more preferably 2 to 12. This shifts the peak temperature of the loss tangent tanδ to a higher temperature after S-UV irradiation, thereby tending to shift the point at which the viscoelastic viscosity of the adhesive increases from the low temperature side to the room temperature side. As a result, destruction of crosslinking points that could serve as the starting point for needle-like cracks is suppressed, and good adhesion to display component members is achieved. In other words, the occurrence of needle-like cracks can be more effectively suppressed, resulting in better weather resistance.

[0049] The adhesive strength of the adhesive layer of the adhesive sheet according to this embodiment after application to soda-lime glass is preferably 1 to 100 N / 25 mm, more preferably 6 to 75 N / 25 mm, particularly preferably 12 to 50 N / 25 mm, even more preferably 20 to 40 N / 25 mm, and most preferably 25 to 38 N / 25 mm. This tends to result in excellent weather resistance and blister resistance. The adhesive strength is basically measured using a 180-degree peel method in accordance with JIS Z0237:2009, and the specific test method is as shown in the test examples described below.

[0050] The total light transmittance of the pressure-sensitive adhesive layer after lamination in the pressure-sensitive adhesive sheet according to this embodiment is preferably 80% or more, more preferably 90% or more, particularly preferably 95% or more, and even more preferably 99% or more. This results in extremely high transparency and makes the sheet suitable for optical applications (for displays). The upper limit of the total light transmittance is not particularly limited, and may be 100%, or may be a value slightly exceeding 100% due to measurement constraints. It is preferable that the total light transmittance of the pressure-sensitive adhesive layer after S-UV irradiation also falls within the same numerical range as that of the pressure-sensitive adhesive layer after lamination. The total light transmittance in this specification is a value measured in accordance with JIS K7361-1:1997, and specific test methods are as shown in the test examples described below.

[0051] The haze value of the pressure-sensitive adhesive layer after lamination in the pressure-sensitive adhesive sheet according to this embodiment is preferably 2% or less, and particularly preferably 1% or less. This provides very high transparency and makes the sheet suitable for optical applications (for displays). The lower limit of the haze value is not particularly limited and may be 0%. It is also preferable that the haze value of the pressure-sensitive adhesive layer after S-UV irradiation is in the same numerical range as that of the pressure-sensitive adhesive layer after lamination. The haze value in this specification is a value measured in accordance with JIS K7136:2000, and specific test methods are as shown in the test examples described below.

[0052] The chromaticity b* (chromaticity b*1) of the pressure-sensitive adhesive layer after lamination in the pressure-sensitive adhesive sheet according to this embodiment, as defined by the CIE 1976 L*a*b* color system, is preferably −20 to 20, more preferably −10 to 10, particularly preferably −5 to 5, even more preferably −2 to 2, and most preferably −1 to 1. This makes the pressure-sensitive adhesive layer nearly colorless and transparent, making it suitable for optical applications.

[0053] The chromaticity b* (chromaticity b*2) of the pressure-sensitive adhesive layer after lamination and S-UV irradiation, as defined by the CIE 1976 L*a*b* color system, is preferably −20 to 20, more preferably −10 to 10, particularly preferably −6 to 6, even more preferably −2 to 2, and most preferably −1 to 1. This means that the pressure-sensitive adhesive layer has a small degree of yellowness even after S-UV irradiation, and is excellent in weather resistance from the standpoint of chromaticity.

[0054] The absolute value of the ratio (b*2 / b*1) of the chromaticity b*2 to the chromaticity b*1 is preferably 20 or less, more preferably 15 or less, particularly preferably 10 or less, even more preferably 5 or less, and most preferably 2 or less. This reduces the degree of yellowing of the pressure-sensitive adhesive layer even after S-UV irradiation, and can be said to have excellent weather resistance from the perspective of chromaticity. The lower limit of the absolute value of the ratio (b*2 / b*1) is not particularly limited, but is most preferably 1.

[0055] The type of adhesive constituting the adhesive layer in this embodiment may be any of an acrylic adhesive, a polyester adhesive, a polyurethane adhesive, a rubber adhesive, a silicone adhesive, etc. The adhesive may be any of an emulsion type, a solvent type, or a solventless type, and may be either a crosslinked type or a non-crosslinked type. Among these, an acrylic adhesive is preferred because of its excellent adhesive properties, optical properties, etc.

[0056] The acrylic pressure-sensitive adhesive may be an active energy ray-curable one, an active energy ray-non-curable one, a crosslinkable one, a non-crosslinkable one, or a combination thereof. Among these, an active energy ray-curable acrylic pressure-sensitive adhesive is preferred from the viewpoint of exhibiting excellent blister resistance.

[0057] The adhesive constituting the adhesive layer in this embodiment preferably contains a (meth)acrylic acid ester polymer as a main adhesive agent, and particularly preferably contains a crosslinked (meth)acrylic acid ester polymer. The adhesive constituting the adhesive layer in this embodiment also preferably contains the above-mentioned main adhesive agent and an active energy ray-curable component. The crosslinked (meth)acrylic acid ester polymer is preferably a crosslinked (meth)acrylic acid ester polymer and a crosslinking agent.

[0058] Specifically, the adhesive constituting the adhesive layer in this embodiment is preferably obtained by crosslinking (preferably thermally crosslinking) an adhesive composition (hereinafter sometimes referred to as "adhesive composition P") containing a (meth)acrylic acid ester polymer (A), a crosslinking agent (B), and, if desired, an active energy ray-curable component (C). In this specification, (meth)acrylic acid means both acrylic acid and methacrylic acid. The same applies to other similar terms. Furthermore, the term "polymer" also includes the concept of "copolymer."

[0059] (1) Components (1-1) (Meth)acrylic acid ester polymer (A) The (meth)acrylic acid ester polymer (A) preferably contains a structural unit derived from a (meth)acrylic acid alkyl ester. This allows the polymer to exhibit good adhesiveness. Note that the (meth)acrylic acid alkyl ester does not include the hard monomer described below.

[0060] From the viewpoint of adhesiveness, the (meth)acrylic acid alkyl ester is preferably a (meth)acrylic acid alkyl ester having an alkyl group containing 1 to 20 carbon atoms. Examples of (meth)acrylic acid alkyl esters having an alkyl group containing 1 to 20 carbon atoms include methyl acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, myristyl (meth)acrylate, palmityl (meth)acrylate, and stearyl (meth)acrylate. These may be used alone or in combination of two or more. Among the above, from the viewpoint of further improving adhesiveness, (meth)acrylic acid esters in which the alkyl group has 1 to 14 carbon atoms are preferred, (meth)acrylic acid esters in which the alkyl group has 2 to 10 carbon atoms are more preferred, and (meth)acrylic acid esters in which the alkyl group has 3 to 8 carbon atoms are particularly preferred. Specifically, for example, methyl acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, or isooctyl (meth)acrylate are preferred, and n-butyl acrylate or 2-ethylhexyl acrylate are particularly preferred.

[0061] From the viewpoint of imparting adhesiveness, the (meth)acrylic acid ester polymer (A) preferably contains 99% by mass or less of structural units derived from (meth)acrylic acid alkyl esters, more preferably 96% by mass or less, and particularly preferably 92% by mass or less. When an acid-free adhesive is preferred as the resulting adhesive due to compatibility with the target adherend, the structural units are preferably contained in an amount of 85% by mass or less, more preferably 80% by mass or less, particularly preferably 75% by mass or less, and even more preferably 70% by mass or less. On the other hand, the lower limit is preferably 40% by mass or more, more preferably 48% by mass or more, particularly preferably 54% by mass or more, and even more preferably 60% by mass or more. In addition, if it is preferred that the resulting pressure-sensitive adhesive contain an acid component due to compatibility with the target adherend, etc., it is preferable that the pressure-sensitive adhesive contain the above-mentioned structural unit in an amount of 70% by mass or more, more preferably 75% by mass or more, particularly preferably 80% by mass or more, and even more preferably 85% by mass or more.

[0062] The (meth)acrylic acid ester polymer (A) preferably contains a structural unit derived from a reactive functional group-containing monomer, whereby the reactive functional group derived from the reactive functional group-containing monomer reacts with the crosslinking agent (B) to form a crosslinked structure (three-dimensional network structure), thereby obtaining a pressure-sensitive adhesive having the desired cohesive strength.

[0063] Preferred examples of the reactive group-containing monomer include a monomer having a hydroxyl group in the molecule (hydroxyl group-containing monomer), a monomer having a carboxyl group in the molecule (carboxyl group-containing monomer), a monomer having an amino group in the molecule (amino group-containing monomer), etc. Among these, a hydroxyl group-containing monomer or a carboxyl group-containing monomer, which has excellent reactivity with the crosslinking agent (B), is preferred.

[0064] Examples of hydroxyl group-containing monomers include (meth)acrylic acid hydroxyalkyl esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. Among these, 2-hydroxyethyl (meth)acrylate or 4-hydroxybutyl (meth)acrylate is preferred from the viewpoints of reactivity with the crosslinking agent (B) and copolymerizability with other monomers. These may be used alone or in combination of two or more.

[0065] Examples of carboxyl group-containing monomers include ethylenically unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, itaconic acid, and citraconic acid. Among them, acrylic acid or methacrylic acid is preferred, and acrylic acid is particularly preferred, from the viewpoint of reactivity with the crosslinking agent (B) and copolymerizability with other monomers. These may be used alone or in combination of two or more.

[0066] From the viewpoint of cohesive strength, the content of the structural unit derived from the reactive functional group-containing monomer in the (meth)acrylic acid ester polymer (A) is preferably 1 to 40 mass%, more preferably 3 to 32 mass%, particularly preferably 6 to 26 mass%, and even more preferably 8 to 22 mass%. Among these, when an acid-free PSA is preferred, the content is preferably 12 to 21 mass%, particularly preferably 16 to 20 mass%, and when an acid component-containing PSA is preferred, the content is preferably 9 to 14 mass%.

[0067] The (meth)acrylic acid ester polymer (A) also preferably contains a structural unit derived from a hard monomer having a glass transition temperature (Tg) of 70°C or higher as a homopolymer. The aforementioned reactive functional group-containing monomers are excluded from the hard monomer. This improves the cohesive strength of the resulting PSA, making it easier to achieve excellent blister resistance. In particular, when a structural unit derived from a (meth)acrylic acid ester having an alkyl group with 5 to 8 carbon atoms is contained, the cohesive strength tends to be low, so it is preferable to contain the structural unit derived from the hard monomer. The glass transition temperature (Tg) of the hard monomer as a homopolymer is preferably 75 to 200°C, particularly preferably 80 to 180°C, and even more preferably 90 to 150°C.

[0068] Examples of the hard monomer include methyl methacrylate (Tg 105° C.), isobornyl acrylate (Tg 94° C.), isobornyl methacrylate (Tg 180° C.), adamantyl acrylate (Tg 115° C.), adamantyl methacrylate (Tg 141° C.), etc. These may be used alone or in combination of two or more.

[0069] Among the above hard monomers, methyl methacrylate or isobornyl acrylate is more preferred from the viewpoint of better demonstrating the performance of the hard monomer while preventing adverse effects on other properties such as adhesion, transparency, etc. In particular, methyl methacrylate is preferred from the viewpoint of weather resistance, and isobornyl acrylate, which is a monomer having an alicyclic structure in the molecule (alicyclic structure-containing monomer), is particularly preferred from the viewpoint of adhesion.

[0070] When the (meth)acrylic acid ester polymer (A) contains the structural unit derived from the hard monomer, the content thereof is preferably 1 to 35% by mass, more preferably 4 to 28% by mass, particularly preferably 8 to 22% by mass, and even more preferably 12 to 17% by mass, from the viewpoint of easily exhibiting the desired cohesive strength and viscoelasticity and from the viewpoint of blister resistance.

[0071] The (meth)acrylic acid ester polymer (A) preferably contains a structural unit derived from a monomer having a nitrogen atom in the molecule (nitrogen atom-containing monomer). In particular, when an alicyclic structure-containing monomer, particularly isobornyl acrylate, is used as the hard monomer, it is preferable to contain a structural unit derived from a nitrogen atom-containing monomer. The presence of a structural unit derived from a nitrogen atom-containing monomer can impart a predetermined polarity to the adhesive and improve the adhesiveness.

[0072] As the nitrogen atom-containing monomer, a monomer having a nitrogen-containing heterocycle is preferred from the viewpoint of providing the (meth)acrylic acid ester polymer (A) with appropriate rigidity. Also, from the viewpoint of increasing the degree of freedom of the nitrogen atom-containing monomer-derived portion in the higher-order structure of the pressure-sensitive adhesive constituted, it is preferred that the nitrogen atom-containing monomer does not contain a reactive unsaturated double bond group other than one polymerizable group used in polymerization to form the (meth)acrylic acid ester polymer (A).

[0073] Examples of monomers having a nitrogen-containing heterocycle include N-(meth)acryloylmorpholine, N-vinyl-2-pyrrolidone, N-(meth)acryloylpyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-(meth)acryloylaziridine, aziridinylethyl (meth)acrylate, 2-vinylpyridine, 4-vinylpyridine, 2-vinylpyrazine, 1-vinylimidazole, N-vinylcarbazole, and N-vinylphthalimide. Among these, N-(meth)acryloylmorpholine, which exhibits superior adhesive strength, is preferred, and N-acryloylmorpholine is particularly preferred. These may be used alone or in combination of two or more.

[0074] When the (meth)acrylic acid ester polymer (A) contains a constituent unit derived from a nitrogen atom-containing monomer, the content thereof is preferably 1 to 20 mass%, more preferably 2 to 16 mass%, particularly preferably 3 to 12 mass%, and even more preferably 4 to 8 mass%, from the viewpoint of making it easier to exhibit the desired viscoelasticity and from the viewpoint of better adhesiveness.

[0075] The (meth)acrylic acid ester polymer (A) may contain structural units derived from other monomers, if desired. The other monomers are preferably monomers that do not contain reactive functional groups, so as not to interfere with the action of the reactive group-containing monomer. Examples of such other monomers include (meth)acrylic acid alkoxyalkyl esters such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate, vinyl acetate, and styrene. These may be used alone or in combination of two or more.

[0076] The (meth)acrylic acid ester polymer (A) may be a polymer obtained by solution polymerization, a polymer obtained without a solvent, or an emulsion polymerization. Among these, a solution polymer obtained by solution polymerization is preferred. By using a solution polymer, a high molecular weight polymer can be easily obtained, and the gel fraction change rate described above is more likely to fall within the preferred range.

[0077] The polymerization mode of the (meth)acrylic acid ester polymer (A) may be a random copolymer or a block copolymer.

[0078] The weight-average molecular weight of the (meth)acrylic acid ester polymer (A) is preferably 100,000 to 3,000,000, more preferably 200,000 to 2,000,000, particularly preferably 300,000 to 1,200,000, and even more preferably 400,000 to 800,000. This makes it easier for the gel fraction change rate to fall within the preferred range. Furthermore, it also makes it easier for the polymer to exhibit desired cohesive strength and viscoelasticity, as well as suitable adhesiveness. The weight-average molecular weight in this specification is a value measured by gel permeation chromatography (GPC) in terms of standard polystyrene.

[0079] In the pressure-sensitive adhesive composition P, the (meth)acrylic acid ester polymer (A) may be used alone or in combination of two or more.

[0080] The content of the (meth)acrylic acid ester polymer (A) in the pressure-sensitive adhesive composition P according to this embodiment is preferably 60 to 99.9% by mass, more preferably 70 to 99% by mass, particularly preferably 80 to 98% by mass, and even more preferably 85 to 97% by mass. When an acid-free pressure-sensitive adhesive is preferred, the content is preferably 90 to 96% by mass. When an acid-containing pressure-sensitive adhesive is preferred, the content is preferably 86 to 91% by mass. This makes it easier for the gel fraction change rate to fall within the preferred range.

[0081] (1-2) Crosslinking Agent (B) The crosslinking agent (B) crosslinks the (meth)acrylic acid ester polymer (A) by heating the pressure-sensitive adhesive composition P, thereby enabling the formation of a favorable crosslinked structure having a three-dimensional network structure. This makes it possible to obtain a pressure-sensitive adhesive having predetermined cohesive strength and viscoelasticity, and to easily obtain excellent blister resistance.

[0082] The crosslinking agent (B) may be any agent that reacts with the reactive functional group (hydroxyl group or carboxyl group) of the (meth)acrylic acid ester polymer (A). Examples include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, amine-based crosslinking agents, melamine-based crosslinking agents, aziridine-based crosslinking agents, hydrazine-based crosslinking agents, aldehyde-based crosslinking agents, oxazoline-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, and ammonium salt-based crosslinking agents. When the (meth)acrylic acid ester polymer (A) contains a structural unit derived from a hydroxyl group-containing monomer, it is preferable to use an isocyanate-based crosslinking agent that has excellent reactivity with hydroxyl groups as the crosslinking agent (B). When the (meth)acrylic acid ester polymer (A) contains a structural unit derived from a carboxyl group-containing monomer, it is preferable to use an epoxy-based crosslinking agent that has excellent reactivity with carboxyl groups as the crosslinking agent (B). The crosslinking agent (B) may be used alone or in combination of two or more.

[0083] The isocyanate-based crosslinking agent contains at least a polyisocyanate compound. Examples of polyisocyanate compounds include aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, and xylylene diisocyanate; aliphatic polyisocyanates such as hexamethylene diisocyanate; alicyclic polyisocyanates such as isophorone diisocyanate and hydrogenated diphenylmethane diisocyanate; and biuret and isocyanurate forms thereof, as well as adducts thereof that are reaction products with low-molecular-weight active hydrogen-containing compounds such as ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, and castor oil. Among these, trimethylolpropane-modified aromatic polyisocyanates, particularly trimethylolpropane-modified tolylene diisocyanate or trimethylolpropane-modified xylylene diisocyanate, are preferred from the viewpoint of reactivity with hydroxyl groups.

[0084] Examples of epoxy crosslinking agents include 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-m-xylylenediamine, ethylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane diglycidyl ether, diglycidylaniline, diglycidylamine, etc. Among these, 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane or N,N,N',N'-tetraglycidyl-m-xylylenediamine is preferred from the viewpoint of reactivity with carboxy groups.

[0085] The content of the crosslinking agent (B) in the pressure-sensitive adhesive composition P is preferably 0.001 to 10 parts by mass, more preferably 0.005 to 5 parts by mass, and particularly preferably 0.01 to 1 part by mass, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). When an acid-free pressure-sensitive adhesive is preferred, the content is preferably 0.05 to 0.8 parts by mass, more preferably 0.1 to 0.6 parts by mass. From the viewpoint of weather resistance, the content is preferably 0.2 to 0.4 parts by mass. When an acid-containing pressure-sensitive adhesive is preferred, the content is preferably 0.015 to 0.5 parts by mass, more preferably 0.02 to 0.1 parts by mass. This makes it easier for the gel fraction change rate to fall within the preferred range.

[0086] (1-3) Active Energy Ray-Curable Component (C) When the pressure-sensitive adhesive composition P contains the active energy ray-curable component (C), the resulting pressure-sensitive adhesive becomes active energy ray-curable.

[0087] The active energy ray-curable component (C) is not particularly limited as long as it is a component that can be cured by irradiation with active energy rays and can provide the above-mentioned physical properties, and may be any of a monomer, an oligomer, a polymer, or a mixture thereof. Among them, preferred is a polyfunctional acrylate-based monomer, which makes it easier for the above-mentioned rate of change in gel fraction to fall within the preferred range.

[0088] Examples of polyfunctional acrylate monomers include bifunctional monomers such as 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, neopentyl glycol adipate di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, caprolactone-modified dicyclopentenyl di(meth)acrylate, ethylene oxide-modified phosphate di(meth)acrylate, di(acryloxyethyl)isocyanurate, allylated cyclohexyl di(meth)acrylate, ethoxylated bisphenol A diacrylate, and 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene; trifunctional types such as diglycerol tetra(meth)acrylate and pentaerythritol tetra(meth)acrylate; pentafunctional types such as propionic acid-modified dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide-modified trimethylolpropane tri(meth)acrylate, tris(acryloxyethyl)isocyanurate, and ε-caprolactone-modified tris-(2-(meth)acryloxyethyl)isocyanurate; tetrafunctional types such as diglycerol tetra(meth)acrylate and pentaerythritol tetra(meth)acrylate; pentafunctional types such as propionic acid-modified dipentaerythritol penta(meth)acrylate; and hexafunctional types such as dipentaerythritol hexa(meth)acrylate and caprolactone-modified dipentaerythritol hexa(meth)acrylate. Among the above, from the viewpoint of the blister resistance of the resulting PSA, preferred are polyfunctional acrylate monomers containing an isocyanurate structure in the molecule, such as di(acryloxyethyl)isocyanurate, tris(acryloxyethyl)isocyanurate, and ε-caprolactone-modified tris-(2-(meth)acryloxyethyl)isocyanurate, more preferred are polyfunctional acrylate monomers which are tri- or higher functional and contain an isocyanurate structure in the molecule, and particularly preferred is ε-caprolactone-modified tris-(2-(meth)acryloxyethyl)isocyanurate.These may be used alone or in combination of two or more. Furthermore, from the viewpoint of making it easier for the resulting pressure-sensitive adhesive to exhibit the desired viscoelasticity, the polyfunctional acrylate monomer preferably has a molecular weight of less than 20,000, more preferably less than 10,000, and particularly preferably less than 5,000. Furthermore, from the viewpoint of compatibility with the (meth)acrylic acid ester polymer (A), a polyfunctional acrylate monomer preferably has a molecular weight of less than 1,000.

[0089] When the pressure-sensitive adhesive composition P contains an active energy ray-curable component (C), the content of the active energy ray-curable component (C) is preferably 1 to 50 parts by mass, more preferably 2 to 40 parts by mass, particularly preferably 3 to 30 parts by mass, and even more preferably 4 to 20 parts by mass, per 100 parts by mass of the (meth)acrylic acid ester polymer (A). When an acid-free pressure-sensitive adhesive is preferred as the resulting pressure-sensitive adhesive, the content is preferably 4.5 to 10 parts by mass, more preferably 5 to 8 parts by mass. Furthermore, when an acid-containing pressure-sensitive adhesive is preferred as the resulting pressure-sensitive adhesive, the content is preferably 5 to 16 parts by mass, more preferably 8 to 14 parts by mass. This makes it easier for the gel fraction change rate to fall within the preferred range.

[0090] (1-4) Photopolymerization initiator (D) When the pressure-sensitive adhesive composition P contains the active energy ray-curable component (C) and ultraviolet light is used as the active energy ray, it is preferable that the pressure-sensitive adhesive composition P contains a photopolymerization initiator (D). This makes it possible to efficiently cure the active energy ray-curable component (C) and reduce the polymerization and curing time and the ultraviolet light irradiation dose.

[0091] Examples of the photopolymerization initiator (D) include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin-n-butyl ether, benzoin isobutyl ether, acetophenone, dimethylaminoacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one, 4-(2-hydroxyethoxy)phenyl-2-(hydroxy-2-propyl)ketone, benzophenone, p-phenylbenzophenone, 4,4 Examples of suitable benzoxanthraquinones include 2-methyl-2-hydroxybenzoyl-1-methyl-1-methyl-2-methyl-1 ...

[0092] Among the above, from the viewpoint of suppressing the occurrence of needle-like cracks, phosphine-based photopolymerization initiators such as 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, or a mixture of 1-hydroxycyclohexyl phenyl ketone and benzophenone are particularly preferred, and from the viewpoints of weather resistance and blister resistance, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide or a mixture of benzophenone and 1-hydroxycyclohexyl phenyl ketone are particularly preferred.

[0093] The content of the photopolymerization initiator (D) in the pressure-sensitive adhesive composition P is preferably 1 to 40 parts by mass, more preferably 3 to 30 parts by mass, particularly preferably 6 to 22 parts by mass, and even more preferably 8 to 14 parts by mass, relative to 100 parts by mass of the active energy ray-curable component (C). This makes it easier for the resulting pressure-sensitive adhesive to satisfy the above-mentioned physical properties.

[0094] (1-5) Silane Coupling Agent (E) The pressure-sensitive adhesive composition P preferably further contains a silane coupling agent (E). This improves the adhesion of the resulting pressure-sensitive adhesive to a glass member when the adherend is a glass member. Furthermore, even when the adherend is a plastic plate, the resulting pressure-sensitive adhesive improves the adhesion of the resulting pressure-sensitive adhesive to the plastic plate. This makes it easier to satisfy the above-mentioned physical properties, and makes it easier to obtain excellent blister resistance in the pressure-sensitive adhesive.

[0095] The silane coupling agent (E) is preferably an organosilicon compound having at least one alkoxysilyl group in the molecule, which has good compatibility with the (meth)acrylic acid ester polymer (A) and has optical transparency.

[0096] Examples of such silane coupling agents (E) include polymerizable unsaturated group-containing silicon compounds such as vinyltrimethoxysilane, vinyltriethoxysilane, and methacryloxypropyltrimethoxysilane; silicon compounds having an epoxy structure such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, and 3-mercaptopropyldimethoxymethylsilane; Examples of suitable silicon compounds include hydroxyl group-containing silicon compounds, amino group-containing silicon compounds such as 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane, and 3-isocyanatepropyltriethoxysilane, as well as condensates of at least one of these with alkyl group-containing silicon compounds such as methyltriethoxysilane, ethyltriethoxysilane, methyltrimethoxysilane, and ethyltrimethoxysilane. These may be used alone or in combination of two or more.

[0097] The content of the silane coupling agent (E) in the pressure-sensitive adhesive composition P is preferably 0.01 to 10 parts by mass, more preferably 0.04 to 5 parts by mass, particularly preferably 0.08 to 1 part by mass, even more preferably 0.12 to 0.5 parts by mass, and especially preferably 0.15 to 0.35 parts by mass, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). This allows the composition to exhibit excellent adhesion, and provides excellent weather resistance and blister resistance.

[0098] (1-6) Ultraviolet absorber (F) The pressure-sensitive adhesive composition P preferably further contains an ultraviolet absorber (F), which allows the resulting pressure-sensitive adhesive layer to more effectively suppress the occurrence of needle-like cracks and has better weather resistance.

[0099] Examples of the ultraviolet absorber (F) include compounds such as benzophenones, benzotriazoles, benzoates, benzoxazinones, triazines, phenyl salicylates, cyanoacrylates, and nickel complex salts. Among these, benzophenones or triazines are preferred from the viewpoints of the effect of suppressing needle cracks and compatibility with the (meth)acrylic acid ester polymer (A). These may be used alone or in combination of two or more.

[0100] Examples of the benzophenone compounds include 2,2-dihydroxy-4-methoxybenzophenone, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid hydrate, and 2-hydroxy-4-n-octyloxybenzophenone.

[0101] Examples of the triazine compounds include 2,4-bis[2-hydroxy-4-butoxyphenyl]-6-(2,4-dibutoxyphenyl)-1,3-5-triazine, 2-[4,6-di(2,4-xylyl)-1,3,5-triazin-2-yl]-5-octyloxyphenol, and 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl]-5-[3-(dodecyloxy)-2-hydroxypropoxy]phenol.

[0102] When the pressure-sensitive adhesive composition P contains an ultraviolet absorber (F), the content of the ultraviolet absorber (F) is preferably 0.01 to 10 parts by mass, more preferably 0.04 to 5 parts by mass, particularly preferably 0.08 to 1 part by mass, even more preferably 0.1 to 0.7 parts by mass, and of these, preferably 0.2 to 0.5 parts by mass, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). This makes it easier for the composition to satisfy the above-mentioned physical properties, and results in excellent weather resistance and blister resistance.

[0103] (1-7) Various Additives The pressure-sensitive adhesive composition P may contain, if desired, various additives commonly used in acrylic pressure-sensitive adhesives, such as a light stabilizer, an oxygen absorber, an antioxidant, a tackifier, a softener, a colorant, an infrared absorber, a rust inhibitor, an antistatic agent, a filler, a refractive index adjuster, etc.

[0104] (2) Production of adhesive composition The adhesive composition P can be produced by producing a (meth)acrylic acid ester polymer (A), mixing the obtained (meth)acrylic acid ester polymer (A) with a crosslinking agent (B), and adding, as desired, an active energy ray-curable component (C), a photopolymerization initiator (D), a silane coupling agent (E), an ultraviolet absorber (F), additives, etc.

[0105] The (meth)acrylic acid ester polymer (A) can be produced by polymerizing a mixture of monomers constituting the polymer by a conventional radical polymerization method. The polymerization of the (meth)acrylic acid ester polymer (A) is preferably carried out by a solution polymerization method using a polymerization initiator as desired. However, the present invention is not limited thereto, and the polymerization may be carried out in the absence of a solvent.

[0106] Examples of polymerization solvents include ethyl acetate, n-butyl acetate, isobutyl acetate, toluene, acetone, hexane, and methyl ethyl ketone, and two or more of these may be used in combination. Examples of polymerization initiators include azo compounds and organic peroxides, and two or more of these may be used in combination. In the polymerization step, the weight-average molecular weight of the resulting polymer can be adjusted by adding a chain transfer agent such as 2-mercaptoethanol.

[0107] Once the (meth)acrylic acid ester polymer (A) is obtained, the crosslinking agent (B), and optionally the active energy ray-curable component (C), the photopolymerization initiator (D), the silane coupling agent (E), the ultraviolet absorber (F), additives, the dilution solvent, etc. are added to the solution of the (meth)acrylic acid ester polymer (A), and mixed thoroughly to obtain a solvent-diluted adhesive composition P (coating solution). Note that when a solid component is used for any of the above components, or when precipitation occurs when mixed with other components in an undiluted state, that component may be dissolved or diluted alone in a dilution solvent before being mixed with other components.

[0108] Examples of the dilution solvent include aliphatic hydrocarbons such as hexane, heptane, and cyclohexane; aromatic hydrocarbons such as toluene and xylene; halogenated hydrocarbons such as methylene chloride and ethylene chloride; alcohols such as methanol, ethanol, propanol, butanol, and 1-methoxy-2-propanol; ketones such as acetone, methyl ethyl ketone, 2-pentanone, isophorone, and cyclohexanone; esters such as ethyl acetate and butyl acetate; and cellosolve-based solvents such as ethyl cellosolve.

[0109] The concentration and viscosity of the coating solution prepared in this manner are not particularly limited as long as they are within a range that allows coating, and can be appropriately selected depending on the situation. For example, the pressure-sensitive adhesive composition P is diluted so that the concentration is 10 to 60 mass %. Note that the addition of a dilution solvent or the like is not a necessary condition for obtaining the coating solution, and as long as the pressure-sensitive adhesive composition P has a viscosity that allows coating, the addition of a dilution solvent is not necessary. In this case, the pressure-sensitive adhesive composition P becomes a coating solution in which the polymerization solvent for the (meth)acrylic acid ester polymer (A) is used as the dilution solvent.

[0110] (3) Production of Pressure-Sensitive Adhesive The pressure-sensitive adhesive composition P described above is applied to a desired object and then crosslinked to obtain a pressure-sensitive adhesive (pressure-sensitive adhesive layer).

[0111] Crosslinking of the pressure-sensitive adhesive composition P can be carried out by a heat treatment. This heat treatment can also serve as a drying treatment after application of the pressure-sensitive adhesive composition P. The heating temperature for the heat treatment is preferably 50 to 150°C, and more preferably 70 to 120°C. The heating time is preferably 10 seconds to 10 minutes, and more preferably 50 seconds to 2 minutes.

[0112] After the heat treatment, a curing period of about 1 to 2 weeks may be provided at room temperature (e.g., 23°C, 50% RH), if necessary. If this curing period is required, the pressure-sensitive adhesive is formed after the curing period has elapsed. If no curing period is required, the pressure-sensitive adhesive is formed after the heat treatment has been completed.

[0113] By the above heat treatment (and curing), a crosslinked product of the (meth)acrylic acid ester polymer (A) crosslinked by the crosslinking agent (B) is formed.

[0114] (4) Thickness of Pressure-Sensitive Adhesive Layer The thickness of the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet according to this embodiment (measured in accordance with JIS K7130) is preferably 1 to 1000 μm, more preferably 10 to 800 μm, and particularly preferably 30 to 600 μm, from the viewpoint of adhesive strength and blister resistance, and is preferably 50 to 400 μm, further preferably 80 to 300 μm, and especially preferably 120 to 260 μm, from the viewpoint of weather resistance.

[0115] (5) Specific Configuration of the Pressure-Sensitive Adhesive Sheet A specific configuration as an example of the pressure-sensitive adhesive sheet according to the present embodiment is shown in Figure 1. As shown in Figure 1, the pressure-sensitive adhesive sheet 1 according to one embodiment is composed of two release sheets 12a, 12b and a pressure-sensitive adhesive layer 11 sandwiched between the two release sheets 12a, 12b so as to be in contact with the release surfaces of the two release sheets 12a, 12b. Note that the release surface of the release sheet in this specification refers to the surface of the release sheet that has releasability, and includes both a surface that has been subjected to a release treatment and a surface that exhibits releasability even without being subjected to a release treatment.

[0116] The pressure-sensitive adhesive layer 11 is the pressure-sensitive adhesive layer in the pressure-sensitive adhesive sheet according to the above-described embodiment.

[0117] The release sheets 12a and 12b protect the adhesive layer until the adhesive sheet is used, and are peeled off when the adhesive sheet (adhesive layer) is to be used. In the adhesive sheet 1 according to this embodiment, one or both of the release sheets 12a and 12b are not necessarily required.

[0118] Examples of materials that can be used as the release sheets 12a and 12b include polyethylene films, polypropylene films, polybutene films, polybutadiene films, polymethylpentene films, polyvinyl chloride films, vinyl chloride copolymer films, polyethylene terephthalate films, polyethylene naphthalate films, polybutylene terephthalate films, polyurethane films, ethylene vinyl acetate films, ionomer resin films, ethylene-(meth)acrylic acid copolymer films, ethylene-(meth)acrylic acid ester polymer films, polystyrene films, polycarbonate films, polyimide films, and fluororesin films. Crosslinked films of these materials can also be used. Furthermore, laminated films of these materials may also be used. From the perspective of the SDGs, the material constituting the release sheets may be a material with a high biomass content, a recyclable or reusable material, or a recycled or reused material.

[0119] It is preferable that a release treatment be performed on the release surfaces of the release sheets 12a and 12b (particularly the surfaces that come into contact with the pressure-sensitive adhesive layer 11). Examples of release agents used for the release treatment include alkyd-based, silicone-based, fluorine-based, unsaturated polyester-based, polyolefin-based, and wax-based release agents.

[0120] There is no particular limitation on the thickness of the release sheets 12a and 12b, but it is usually about 20 to 150 μm.

[0121] From the viewpoint of ease of handling, it is preferable that one of the two release sheets 12a, 12b be a heavy release type release sheet with a large release force and the other be a light release type release sheet with a small release force.

[0122] (6) Production of Pressure-Sensitive Adhesive Sheet In one example of producing the pressure-sensitive adhesive sheet 1, a coating solution of the pressure-sensitive adhesive composition P is applied to the release surface of one release sheet 12a (or 12b), and a heat treatment is carried out to thermally crosslink the pressure-sensitive adhesive composition P to form a coating layer, after which the release surface of the other release sheet 12b (or 12a) is superimposed on the coating layer. If a curing period is required, a curing period is allowed, but if no curing period is required, the coating layer becomes the pressure-sensitive adhesive layer 11 as is. The pressure-sensitive adhesive sheet 1 is obtained by the above steps. The conditions for the heat treatment and curing are as described above.

[0123] The coating solution of the adhesive composition P can be applied by, for example, bar coating, knife coating, roll coating, blade coating, die coating, gravure coating, or the like.

[0124] [Display Body] A display body according to one embodiment of the present invention includes one display body component, another display body component, and an adhesive layer that bonds the one display body component and the other display body component to each other. The adhesive layer is formed from the adhesive layer of the adhesive sheet according to the embodiment described above.

[0125] At least one of the one display member constituting member and the other display member constituting member may have a step at least on the surface on the side to be bonded by the pressure-sensitive adhesive layer.

[0126] Both the first display member and the second display member may be hard plates. When two hard plates are to be bonded together, since the hard plates are hard and inflexible, the adhesive layer is attached to one of the hard plates, and the two hard plates are pressed vertically to bring the adhesive layer into close contact with each other, thereby bonding the two hard plates together.

[0127] A display according to one embodiment of the present invention will be described with reference to the drawings. As shown in Fig. 2, the display 2 according to this embodiment is configured to include a first display component 21 (one display component), a second display component 22 (another display component), and an adhesive layer 11 positioned therebetween to bond the first display component 21 and the second display component 22 to each other.

[0128] At least one of the first display body component 21 and the second display body component 22 may have a step on at least the surface that is bonded by the adhesive layer 11. In the present embodiment shown in Fig. 2, the first display body component 21 has a step on the surface on the adhesive layer 11 side due to the printing layer 3 or the like.

[0129] The adhesive layer 11 in the display body 2 is either the adhesive layer 11 (non-curable by active energy rays) of the aforementioned adhesive sheet 1 itself, or the adhesive layer 11 (curable by active energy rays) of the aforementioned adhesive sheet 1 that has been cured by irradiation with active energy rays.

[0130] Examples of the display 2 include a liquid crystal (LCD) display, a light-emitting diode (LED) display, an organic electroluminescence (OLED) display, and electronic paper, and may also be a touch panel. Note that LED displays also include those using mini LEDs and micro LEDs.

[0131] The first display member 21 is preferably a protective panel made of a glass plate, a plastic plate, or a laminate containing these. In this case, the printing layer 3 is generally formed in a frame shape on the pressure-sensitive adhesive layer 11 side of the first display member 21.

[0132] The glass plate is not particularly limited, and examples thereof include chemically strengthened glass, alkali-free glass, quartz glass, soda-lime glass, barium-strontium-containing glass, aluminosilicate glass, lead glass, borosilicate glass, barium borosilicate glass, etc. The thickness of the glass plate is not particularly limited, but is usually 0.1 to 5 mm, and preferably 0.2 to 2 mm.

[0133] The plastic plate is not particularly limited, and examples thereof include an acrylic plate, a polycarbonate plate, etc. The thickness of the plastic plate is not particularly limited, but is usually 0.2 to 5 mm, and preferably 0.4 to 3 mm.

[0134] On one or both sides of the glass plate or plastic plate, various functional layers (transparent conductive film, metal layer, silica layer, hard coat layer, anti-glare layer, etc.) may be provided, or optical members may be laminated. Furthermore, the transparent conductive film and metal layer may be patterned.

[0135] The second display component 22 is preferably an optical element to be attached to the first display component 21, a display module (e.g., a liquid crystal (LCD) module, a light-emitting diode (LED) module, an organic electroluminescence (organic EL) module, etc.), an optical element as part of a display module, or a laminate including a display module.

[0136] Examples of the optical member include a shatterproof film, a polarizing plate (polarizing film), a polarizer, a retardation plate (retardation film), a viewing angle compensation film, a brightness improvement film, a contrast improvement film, a liquid crystal polymer film, a diffusion film, a semi-transmitting reflective film, a transparent conductive film, etc. A preferred example of the transparent conductive film is an ITO-PET film in which a tin-doped indium oxide (ITO) layer is formed on one surface of a polyethylene terephthalate film.

[0137] The material constituting the printing layer 3 is not particularly limited, and known materials for printing can be used. The thickness of the printing layer 3, i.e., the height of the step, is preferably 0.5 to 50 μm, more preferably 1 to 30 μm, and particularly preferably 3 to 20 μm. When the thickness of the printing layer 3 is within the above range, the step-following ability of the pressure-sensitive adhesive layer 11 is effectively exhibited, and the concealing property that is the purpose of the printing layer 3 can be sufficiently ensured. Note that the printing layer 3 is generally formed in a frame shape on the pressure-sensitive adhesive layer 11 side of the display component.

[0138] As an example, to manufacture the display body 2, one release sheet 12a of the adhesive sheet 1 is peeled off, and the exposed adhesive layer 11 of the adhesive sheet 1 is attached to the surface of the first display body component 21 on which the printing layer 3 is present.

[0139] Next, the other release sheet 12b is peeled off from the adhesive layer 11 of the adhesive sheet 1, and the exposed adhesive layer 11 of the adhesive sheet 1 is bonded to the second display body component 22 to obtain a display body. As another example, the bonding order of the first display body component 21 and the second display body component 22 may be reversed.

[0140] Here, when the pressure-sensitive adhesive layer 11 is active energy ray-curable (when it contains the active energy ray-curable component (C)), it is preferable to bond the laminate of the first display body component 21 and the pressure-sensitive adhesive layer 11 to the second display body component 22, and then irradiate the pressure-sensitive adhesive layer 11 with active energy rays through the first display body component 21 and / or the second display body component 22 to cure the pressure-sensitive adhesive layer 11. This results in better blister resistance.

[0141] The active energy ray refers to an electromagnetic wave or a charged particle beam that has an energy quantum, and specific examples thereof include ultraviolet rays, electron beams, etc. Among active energy rays, ultraviolet rays are particularly preferred because they are easy to handle.

[0142] The ultraviolet irradiation can be performed using a high-pressure mercury lamp, a Heraeus H lamp, a xenon lamp, or the like, and the amount of ultraviolet irradiation is set to an illuminance of 50 to 1000 mW / cm. 2 The light intensity is preferably about 50 to 10,000 mJ / cm. 2 is preferably 80 to 5000 mJ / cm 2 More preferably, it is 300 to 2000 mJ / cm 2 On the other hand, the electron beam irradiation can be carried out by an electron beam accelerator or the like, and the irradiation dose of the electron beam is preferably about 10 to 1000 krad.

[0143] In the display body 2, the adhesive constituting the adhesive layer 11 has the physical properties described above, so even when exposed to high-intensity ultraviolet light for a long period of time (for example, 20 hours, 40 hours, or in some cases 80 hours), the occurrence of needle-like cracks in the adhesive layer 11 is suppressed, and the display body 2 has excellent weather resistance.

[0144] The above-described embodiments have been described to facilitate understanding of the present invention, and are not intended to limit the present invention. Therefore, each element disclosed in the above embodiments is intended to include all design modifications and equivalents that fall within the technical scope of the present invention.

[0145] For example, one or both of the release sheets 12a and 12b in the pressure-sensitive adhesive sheet 1 may be omitted, or a desired optical member may be laminated in place of the release sheets 12a and / or 12b. The first display body component 21 may not have a step. Furthermore, not only the first display body component 21 but also the second display body component 22 may have a step on the pressure-sensitive adhesive layer 11 side.

[0146] In this specification, when it is stated that "X to Y" (X and Y are any numbers), it means "X or more and Y or less" unless otherwise specified, and also means "preferably greater than X" or "preferably smaller than Y". Furthermore, when it is stated that "X or more" (X is any number), it means "preferably greater than X" unless otherwise specified, and when it is stated that "Y or less" (Y is any number), it also means "preferably smaller than Y" unless otherwise specified.

[0147] The present invention will be explained in more detail below with reference to examples, but the scope of the present invention is not limited to these examples.

[0148] Example 1 1. Preparation of (meth)acrylic acid ester polymer 60 parts by mass of 2-ethylhexyl acrylate, 20 parts by mass of methyl methacrylate, and 20 parts by mass of 2-hydroxyethyl acrylate were copolymerized by solution polymerization to prepare a (meth)acrylic acid ester polymer (A). The molecular weight of this (meth)acrylic acid ester polymer (A) was measured by the method described below, and the weight average molecular weight (Mw) was found to be 700,000.

[0149] 2. Preparation of adhesive composition 100 parts by mass (solid content equivalent; the same applies hereinafter) of the (meth)acrylic acid ester polymer (A) obtained in step 1 above, 0.25 parts by mass of an isocyanate-based crosslinking agent (B1; manufactured by Mitsui Chemicals, Inc., product name "Takenate D-101E"), and 0.27 parts by mass of 3-glycidoxypropyltrimethoxysilane as a silane coupling agent (E) were mixed, thoroughly stirred, and diluted with methyl ethyl ketone to obtain a coating solution of an adhesive composition.

[0150] Here, the formulations (solid content equivalent) of the pressure-sensitive adhesive compositions when the (meth)acrylic acid ester polymer (A) is taken as 100 parts by mass (solid content equivalent) are shown in Table 1. Details of the abbreviations and the like shown in Table 1 are as follows. [(Meth)acrylic acid ester polymer (A)] 2EHA: 2-ethylhexyl acrylate BA: n-butyl acrylate MMA: methyl methacrylate IBXA: isobornyl acrylate ACMO: N-acryloylmorpholine HEA: 2-hydroxyethyl acrylate AA: acrylic acid [Crosslinking agent (B)] B1: isocyanate-based crosslinking agent (manufactured by Mitsui Chemicals, Inc., product name "Takenate D-101E") B2: 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane (epoxy-based crosslinking agent) [Photopolymerization initiator (D)] D1: mixture of 1-hydroxycyclohexyl phenyl ketone and benzophenone (mass ratio 50:50) D2: 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide D3: bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide D4: 1-Hydroxycyclohexylphenyl ketone D5: Mixture of 2-oxy-2-phenylacetic acid-2-(2-oxo-2-phenylacetoxyethoxy)ethyl ester and 2-oxy-2-phenylacetic acid-2-(2-hydroxyethoxy)ethyl ester (manufactured by IGM Resins, product name "OMNIRAD 754") [UV absorber (F)] F1: 2,2-dihydroxy-4-methoxybenzophenone F2: 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl]-5-[3-(dodecyloxy)-2-hydroxypropoxy]phenol

[0151] 3. Manufacturing of Pressure-Sensitive Adhesive Sheet The coating solution of the pressure-sensitive adhesive composition obtained in step 2 above was applied using a coater to the release-treated surface of a heavy-release type release sheet R1, which had been prepared by treating one side of a polyethylene terephthalate film with a silicone-based release agent. A coating layer was then formed by heating at 90°C for 1 minute. The coating layer on the release sheet R1 obtained above was then attached to a light-release type release sheet R2, which had been prepared by treating one side of a polyethylene terephthalate film with a silicone-based release agent, so that the release-treated surface of the release sheet R2 was in contact with the coating layer. This was then cured for 7 days under conditions of 23°C and 50% RH to produce a pressure-sensitive adhesive sheet having a thickness of 50 μm, i.e., a pressure-sensitive adhesive sheet having a configuration of release sheet R1 / adhesive layer (thickness: 50 μm) / release sheet R2. The pressure-sensitive adhesive layer in this pressure-sensitive adhesive sheet was not curable by active energy rays.

[0152] The thickness of the pressure-sensitive adhesive layer was measured using a constant pressure thickness measuring device (manufactured by Teclock Corporation, product name "PG-02") in accordance with JIS K 7130. Furthermore, it was confirmed that the release strength of release sheet R1 was greater than that of release sheet R2 in the obtained pressure-sensitive adhesive sheet.

[0153] Example 2 A pressure-sensitive adhesive sheet was produced in the same manner as in Example 1, except that, in preparing the pressure-sensitive adhesive composition, 5.2 parts by mass of ε-caprolactone-modified tris-(2-acryloxyethyl)isocyanurate (manufactured by Shin-Nakamura Chemical Co., Ltd., product name "NK Ester A-9300-1CL") as the active energy ray-curable component (C) and 0.5 parts by mass of a mixture of 1-hydroxycyclohexyl phenyl ketone and benzophenone (mass ratio 50:50) (D1) as the photopolymerization initiator (D) were further blended. Note that the pressure-sensitive adhesive layer in this pressure-sensitive adhesive sheet was active energy ray-curable.

[0154] Examples 3 to 8, Comparative Examples 1 to 3 Pressure-sensitive adhesive sheets were produced in the same manner as in Example 2, except that the type and weight-average molecular weight (Mw) of each monomer constituting the (meth)acrylic acid ester polymer (A), the type and amount of crosslinking agent (B), the amount of active energy ray-curable component (C), and the type and amount of photopolymerization initiator (D) were changed as shown in Table 1. In Examples 5 and 6, ultraviolet absorbers (F1 / F2) were further added in the amounts shown in Table 1.

[0155] The weight average molecular weight (Mw) is a polystyrene-equivalent weight average molecular weight measured by gel permeation chromatography (GPC) under the following conditions (GPC measurement). <Measurement conditions> Measurement device: HLC-8320, manufactured by Tosoh Corporation GPC columns (passed in the following order): TSK gel super H-H, TSK gel super HM-H, TSK gel super H2000, manufactured by Tosoh Corporation Measurement solvent: tetrahydrofuran Measurement temperature: 40°C

[0156] [Test Example 1] (Measurement of gel fraction) A 250 μm thick adhesive layer was prepared by laminating multiple adhesive layers of the adhesive sheets produced in the Examples and Comparative Examples. The adhesive layer (thickness: 250 μm) was cut to a size of 70 mm × 150 mm, and the adhesive layer was wrapped in a polyester mesh (mesh size 200). The mass was weighed using a precision balance, and the mass of the mesh alone was subtracted to calculate the mass of the adhesive alone. This mass was designated M1.

[0157] Next, the adhesive wrapped in the polyester mesh was immersed in ethyl acetate at room temperature (23°C) for 24 hours. The adhesive was then removed and air-dried for 24 hours in an environment at 23°C and 50% RH, and then dried in an oven at 80°C for 12 hours. After drying, the mass was weighed using a precision balance, and the mass of the mesh alone was subtracted to calculate the mass of the adhesive alone. This mass was designated M2. The gel fraction (%; before UV) was expressed as (M2 / M1) x 100. In Example 1 (non-active energy ray curable), the gel fraction (before UV) was G1, while in Examples other than Example 1 and Comparative Examples (active energy ray curable), the gel fraction (before UV) was G0. The results are shown in Table 2.

[0158] Furthermore, a 250 μm thick adhesive layer was produced by laminating multiple adhesive layers from the adhesive sheets produced in the Examples (other than Example 1) and Comparative Examples. The adhesive layer (thickness: 250 μm) was irradiated with active energy rays (ultraviolet rays; UV) to cure the adhesive layer. The gel fraction (%; after UV) of the adhesive in the adhesive layer after curing with the active energy rays was measured in the same manner as above. In Examples and Comparative Examples other than Example 1, the gel fraction (after UV) was G1. The results are shown in Table 2. The irradiation conditions for active energy rays were as follows:

[0159] <Activated energy ray irradiation conditions> - High pressure mercury lamp used - Illuminance: 200 mW / cm 2 , Light amount: 1000mJ / cm 2 ・UV illuminance and light intensity meter used is "UVPF-A1" manufactured by iGraphics

[0160] Furthermore, a 250 μm thick adhesive layer was prepared by laminating multiple adhesive layers from the adhesive sheets prepared in the Examples and Comparative Examples. Using this adhesive layer (thickness: 250 μm), two soda-lime glass plates (manufactured by Nippon Sheet Glass Co., Ltd., thickness: 1.1 mm, length: 70 mm × width: 150 mm) were bonded to prepare a laminate (soda-lime glass plate / adhesive layer (250 μm) / soda-lime glass plate). The laminates of the Examples (other than Example 1) and Comparative Examples were irradiated with active energy rays (ultraviolet rays; UV) under the above-mentioned active energy ray irradiation conditions to cure the adhesive layer. As a result, the laminate of Example 1, which had a non-active energy ray-curable adhesive layer, and the laminates of the Examples (other than Example 1) and Comparative Examples, which had an active energy ray-cured adhesive layer, were obtained.

[0161] The obtained laminate was irradiated with ultraviolet light (S-UV irradiation) under the following conditions. Then, for the laminate after S-UV irradiation, the pressure-sensitive adhesive layer was separated from the two soda-lime glass plates. For the pressure-sensitive adhesive of the pressure-sensitive adhesive layer after separation, the gel fraction (%; G2) was measured in the same manner as above. The results are shown in Table 2.

[0162] <Ultraviolet light irradiation conditions> Device: Eye Super UV Tester SUV-W151 (manufactured by Iwasaki Electric Co., Ltd.) UV lamp: ME06-L31WX / SUV (manufactured by Iwasaki Electric Co., Ltd.) Water-cooled jacket: WJ50-SUV-4 (manufactured by Iwasaki Electric Co., Ltd.) Illuminance: 100 mW / cm 2 Irradiation time: 120 hours Light intensity: 43.2 kJ / cm 2 Temperature: 63°C Humidity: 70% RH Temperature and humidity control: Closed circulation method

[0163] Based on the G1 and G2 obtained above, the gel fraction change rate ((G2 / G1)×100) (%), which is the ratio of G2 to G1, was calculated. The results are shown in Table 2.

[0164] [Test Example 2] (Measurement of the average peak molecular weight of the sol component) A plurality of pressure-sensitive adhesive layers of the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples were laminated together to produce a pressure-sensitive adhesive layer having a thickness of 250 μm. Except for Example 1, the pressure-sensitive adhesive layer (250 μm) was irradiated with active energy rays (ultraviolet rays; UV) under the same active energy ray irradiation conditions as in Test Example 1, and the pressure-sensitive adhesive layer was cured.

[0165] For the non-active energy ray-curable pressure-sensitive adhesive layer (250 μm) of Example 1 obtained as above, and the active energy ray-cured pressure-sensitive adhesive layers (250 μm) of Examples (other than Example 1) and Comparative Examples, ethyl acetate (after immersion in the pressure-sensitive adhesive and removal) obtained in the same manner as in Test Example 1 was concentrated in an evaporator to obtain a sol. The sol was then diluted with tetrahydrofuran to a 0.3 mass% solution, filtered through a 0.45 μm filter, and the average peak molecular weight (Mp; before S-UV) of the sol was measured by GPC measurement. The measurement conditions for the GPC measurement were as described above. The results are shown in Table 2.

[0166] Furthermore, a 250 μm thick adhesive layer was produced by laminating multiple adhesive layers from the adhesive sheets produced in the Examples and Comparative Examples. Using this adhesive layer (thickness: 250 μm), a laminate was produced in the same manner as in Test Example 1. The laminates of the Examples (other than Example 1) and Comparative Examples were irradiated with active energy rays (ultraviolet rays; UV) under the same active energy ray irradiation conditions as in Test Example 1 to cure the adhesive layer. As a result, the laminate of Example 1, which had a non-active energy ray-curable adhesive layer, and the laminates of the Examples (other than Example 1) and Comparative Examples, which had an active energy ray-cured adhesive layer, were obtained.

[0167] The obtained laminate was irradiated with ultraviolet light (S-UV irradiation) under the same ultraviolet irradiation conditions as in Test Example 1. Then, for the laminate after S-UV irradiation, the pressure-sensitive adhesive layer was separated from the two soda-lime glass plates. For the pressure-sensitive adhesive in the pressure-sensitive adhesive layer after separation, the average peak molecular weight (Mp; after S-UV) of the sol component was measured in the same manner as above. The results are shown in Table 2.

[0168] [Test Example 3] (Measurement of dynamic viscoelasticity) A pressure-sensitive adhesive layer having a thickness of 250 μm was prepared by laminating multiple pressure-sensitive adhesive layers of the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples. Except for Example 1, the pressure-sensitive adhesive layer (250 μm) was irradiated with active energy rays (ultraviolet rays; UV) under the same active energy ray irradiation conditions as in Test Example 1, and the pressure-sensitive adhesive layer was cured.

[0169] From the non-active energy ray-curable pressure-sensitive adhesive layer (250 μm) of Example 1 obtained as described above, and the active energy ray-cured pressure-sensitive adhesive layers (250 μm) of the Examples (other than Example 1) and Comparative Examples, cylindrical bodies with a diameter of 8 mm (height 0.25 mm) were punched out and used as samples.

[0170] The dynamic viscoelasticity of the above sample was measured in accordance with JIS K7244-1 using a viscoelasticity measuring device (manufactured by Anton Paar, product name "MCR302") by the torsional shear method under the following conditions, and the storage modulus G'(-15) (MPa; before S-UV) at -15°C, the storage modulus G'(23) (MPa; before S-UV) at 23°C, and the storage modulus G'(100) (MPa; before S-UV) at 100°C were calculated. In addition, the peak temperature (°C) of the loss tangent tanδ (before S-UV: Tb) was calculated. The results are shown in Table 2. Measurement frequency: 1 Hz Measurement temperature range: -20°C to 140°C Heating rate: 4°C / min

[0171] Furthermore, a 250 μm thick adhesive layer was produced by laminating multiple adhesive layers from the adhesive sheets produced in the Examples and Comparative Examples. Using this adhesive layer (thickness: 250 μm), a laminate was produced in the same manner as in Test Example 1. The laminates of the Examples (other than Example 1) and Comparative Examples were irradiated with active energy rays (ultraviolet rays; UV) under the same active energy ray irradiation conditions as in Test Example 1 to cure the adhesive layer. As a result, the laminate of Example 1, which had a non-active energy ray-curable adhesive layer, and the laminates of the Examples (other than Example 1) and Comparative Examples, which had an active energy ray-cured adhesive layer, were obtained.

[0172] The obtained laminate was irradiated with ultraviolet light under the same ultraviolet irradiation conditions as in Test Example 1 (S-UV irradiation). Then, for the laminate after S-UV irradiation, the pressure-sensitive adhesive layer was separated from the two soda-lime glass plates. For the pressure-sensitive adhesive layer after separation, the dynamic viscoelasticity was measured in the same manner as above, and the storage modulus G'(-15) (MPa; after S-UV) at -15°C, the storage modulus G'(23) (MPa; after S-UV) at 23°C, and the storage modulus G'(100) (MPa; after S-UV) at 100°C were observed. In addition, the peak temperature (°C) of the loss tangent tanδ (after S-UV: Ta) was also observed. The results are shown in Table 2.

[0173] Furthermore, the value (Ta - Tb) was calculated by subtracting Tb from Ta obtained above. The results are shown in Table 2.

[0174] [Test Example 4] (Measurement of adhesive strength) The release sheet R2 was peeled off from the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples, and the exposed pressure-sensitive adhesive layer was attached to one of the easy-adhesion layers of a polyethylene terephthalate (PET) film (manufactured by Toyobo Co., Ltd., product name "Cosmoshine A4360", thickness: 100 μm) having easy-adhesion layers on both sides, to obtain a release sheet R1 / adhesive layer / PET film laminate. The laminate was cut into a 25 mm wide, 100 mm long sample.

[0175] The release sheet R1 was peeled off from the sample in an environment of 23°C and 50% RH, and the exposed pressure-sensitive adhesive layer was attached to soda lime glass (manufactured by Nippon Sheet Glass Co., Ltd.), and then pressurized for 20 minutes at 0.5 MPa and 50°C in an autoclave manufactured by Kurihara Manufacturing Co., Ltd. For the examples (other than Example 1) and comparative examples, active energy rays (ultraviolet rays; UV) were irradiated through the soda lime glass under the same active energy ray irradiation conditions as in Test Example 1, to cure the pressure-sensitive adhesive layer.

[0176] After that, the adhesive strength (N / 25 mm) was measured using a tensile tester (Tensilon, manufactured by Orientec Co., Ltd.) at a peel speed of 300 mm / min and a peel angle of 180 degrees. The measurement was conducted under conditions other than those described here in accordance with JIS Z0237:2009. The results are shown in Table 2.

[0177] [Test Example 5] (Measurement of total light transmittance) A pressure-sensitive adhesive layer having a thickness of 250 μm was prepared by laminating multiple pressure-sensitive adhesive layers of the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples. A laminate was prepared using this pressure-sensitive adhesive layer (thickness: 250 μm) in the same manner as in Test Example 1. For Example 1, this laminate was used as a measurement sample. For the Examples (other than Example 1) and Comparative Examples, the laminate was irradiated with active energy rays (ultraviolet rays; UV) under the same active energy ray irradiation conditions as in Test Example 1 to cure the pressure-sensitive adhesive layer, and this was used as a measurement sample.

[0178] For the measurement sample, background measurement was performed using soda lime glass, and then the total light transmittance (%; before S-UV) was measured using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "NDH-5000") in accordance with JIS K7361-1:1997. The results are shown in Table 2. The total light transmittance of the pressure-sensitive adhesive layer before curing with active energy rays was also measured, and the same measurement results were obtained.

[0179] Test Example 6 (Haze Value Measurement) A measurement sample was prepared in the same manner as in Test Example 5. After background measurement was performed on the measurement sample using glass, the haze value (%; before S-UV) was measured using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "NDH-5000") in accordance with JIS K7136:2000. The results are shown in Table 2. The haze value of the pressure-sensitive adhesive layer before curing with active energy rays was also measured, and the same measurement result was obtained.

[0180] [Test Example 7] (Measurement of L*a*b*) A 250 μm thick pressure-sensitive adhesive layer was produced by laminating multiple pressure-sensitive adhesive layers from the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples. Using this pressure-sensitive adhesive layer (thickness: 250 μm), a laminate was produced in the same manner as in Test Example 1. The laminates of the Examples (other than Example 1) and Comparative Examples were irradiated with active energy rays (ultraviolet rays; UV) under the same active energy ray irradiation conditions as in Test Example 1 to cure the pressure-sensitive adhesive layer. As a result, the laminate of Example 1, which had a non-active energy ray-curable pressure-sensitive adhesive layer, and the laminates of the Examples (other than Example 1) and Comparative Examples, which had an active energy ray-cured pressure-sensitive adhesive layer, were obtained.

[0181] The chromaticity b* (chromaticity b*1) of the obtained laminate was measured using a simultaneous spectrophotometric colorimeter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "SQ2000") according to the CIE 1976 L*a*b* color system. The results are shown in Table 2.

[0182] The obtained laminate was also irradiated with ultraviolet light (S-UV irradiation) under the same ultraviolet irradiation conditions as in Test Example 1. The chromaticity b* (chromaticity b*2) of the pressure-sensitive adhesive layer after S-UV irradiation was measured in the same manner as above. The results are shown in Table 2.

[0183] Furthermore, the absolute value of the ratio (b*2 / b*1) of the chromaticity b*2 to the chromaticity b*1 obtained above was calculated. The results are shown in Table 2.

[0184] [Test Example 8] (Evaluation of Weather Resistance) A 250 μm thick pressure-sensitive adhesive layer was produced by laminating multiple pressure-sensitive adhesive layers from the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples. Using this pressure-sensitive adhesive layer (thickness: 250 μm), a laminate was produced in the same manner as in Test Example 1. For the laminates of the Examples (other than Example 1) and Comparative Examples, active energy rays (ultraviolet rays; UV) were irradiated under the same active energy ray irradiation conditions as in Test Example 1 to cure the pressure-sensitive adhesive layer. As a result, the laminate of Example 1, which had a non-active energy ray-curable pressure-sensitive adhesive layer, and the laminates of the Examples (other than Example 1) and Comparative Examples, which had an active energy ray-cured pressure-sensitive adhesive layer, were obtained.

[0185] Next, the obtained laminate was irradiated with ultraviolet light for 20 hours (light amount: 7.2 kJ / cm 2 ), 40 hours (light intensity: 14.4 kJ / cm 2 ), 80 hours (light intensity: 28.8 kJ / cm 2 The adhesive layer was then visually inspected and its weather resistance was evaluated based on the following criteria. The results are shown in Table 2. ⊚: No needle-like cracks occurred, and no bubbles, lifting, or peeling occurred. ◯: No needle-like cracks occurred, but some bubbles occurred. ×: Needle-like cracks occurred.

[0186] Test Example 9 (Evaluation of Blister Resistance) The release sheet R2 was peeled off from the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples, and the exposed pressure-sensitive adhesive layer was bonded to the PC plate side of a plastic plate (manufactured by Mitsubishi Gas Chemical Company, Inc., product name "Iupilon Sheet MR58U", thickness: 0.7 mm) consisting of a polycarbonate (PC) plate and a polymethyl methacrylate (PMMA) layer laminated thereon. The release sheet R1 was then peeled off from the pressure-sensitive adhesive layer to expose the pressure-sensitive adhesive layer, and a transparent conductive film (manufactured by Oike Kogyo Co., Ltd., laminate of a PET film and an ITO layer (ITO-PET film), total thickness 125 μm) was bonded to the pressure-sensitive adhesive layer so that the ITO layer side was in contact with the pressure-sensitive adhesive layer. The sheet was then autoclaved for 20 minutes at 50°C and 0.5 MPa.

[0187] For Example 1, after the autoclave treatment, the laminate was left to stand for 24 hours at normal pressure, 23°C, and 50% RH, and this was used as a sample. For Examples and Comparative Examples other than Example 1, the pressure-sensitive adhesive layer of the laminate obtained above was irradiated with active energy rays (ultraviolet rays; UV) through the transparent conductive film under the same conditions as in Test Example 1, to cure the pressure-sensitive adhesive layer. Thereafter, the laminate was left to stand for 24 hours at normal pressure, 23°C, and 50% RH, and this was used as a sample.

[0188] The obtained sample was stored under high temperature and high humidity conditions of 85°C and 85% RH for 72 hours. Thereafter, the condition of the interface between the pressure-sensitive adhesive layer and the adherend (plastic plate) was visually inspected, and blister resistance was evaluated according to the following criteria. The results are shown in Table 2. ○: No bubbles, lifting, or peeling occurred. △: Bubbles less than 1 mm in diameter occurred, but no lifting or peeling occurred. ×: Bubbles, lifting, or peeling occurred throughout the sample.

[0189]

[0190]

[0191] As can be seen from Table 2, the PSA sheets produced in the examples were able to suppress the occurrence of needle-like cracks even when irradiated with high-intensity ultraviolet light for long periods of time (20 hours / 40 hours), and were therefore excellent in weather resistance. In particular, the PSA sheets produced in Examples 1 and 5 to 8 were able to suppress the occurrence of needle-like cracks even when irradiated with high-intensity ultraviolet light for even longer periods of time (80 hours), and were therefore even more excellent in weather resistance.

[0192] The pressure-sensitive adhesive sheet of the present invention can be suitably used, for example, in the production of a display, for bonding a display component such as a protective panel to a desired display component.

[0193] DESCRIPTION OF SYMBOLS 1... Adhesive sheet 11... Adhesive layer 12a, 12b... Release sheets 2... Display body 21... First display body constituent member 22... Second display body constituent member 3... Printed layer

Claims

1. An adhesive sheet having an adhesive layer for bonding two display component members to each other, the gel fraction of the adhesive constituting the adhesive layer after the bonding is G1, and the illuminance of the adhesive layer after the bonding is 100 mW / cm 2 a gel fraction of an adhesive constituting the adhesive layer after irradiation with ultraviolet light of 100 nm for 120 hours is defined as G2, wherein G1 is 30% or more and 95% or less, and a gel fraction change rate, which is a ratio of G2 to G1, is 117% or less.

2. The adhesive sheet according to claim 1, characterized in that the average peak molecular weight of the sol component of the adhesive constituting the adhesive layer after lamination is 10,000 or more and 250,000 or less.

3. Illuminance of the adhesive layer after lamination: 100 mW / cm 2 2. The pressure-sensitive adhesive sheet according to claim 1, characterized in that after being irradiated with ultraviolet light of 10,000 for 120 hours, the average peak molecular weight of the sol component of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer is 10,000 or more and 200,000 or less.

4. The pressure-sensitive adhesive sheet according to claim 1, characterized in that the storage modulus G' at 23° C. of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer after lamination is 0.01 MPa or more and 2 MPa or less.

5. Illuminance of the adhesive layer after lamination: 100 mW / cm 2 2. The pressure-sensitive adhesive sheet according to claim 1, wherein the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer has a storage modulus G' at 23°C of 0.01 MPa or more and 2 MPa or less after being irradiated with ultraviolet light of 1000 nm for 120 hours.

6. The pressure-sensitive adhesive sheet according to claim 1, wherein the storage modulus G' of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer after lamination is 0.01 MPa or more and 100 MPa or less at -15°C.

7. Illuminance of the adhesive layer after lamination: 100 mW / cm 2 2. The pressure-sensitive adhesive sheet according to claim 1, wherein the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer has a storage modulus G' at -15°C of 0.1 MPa or more and 1000 MPa or less after being irradiated with ultraviolet light of 1000 nm for 120 hours.

8. The pressure-sensitive adhesive sheet according to claim 1, characterized in that the storage modulus G' at 100° C. of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer after lamination is 0.0001 MPa or more and 1 MPa or less.

9. Illuminance of the adhesive layer after lamination: 100 mW / cm 2 2. The pressure-sensitive adhesive sheet according to claim 1, wherein the pressure-sensitive adhesive layer has a storage modulus G' at 100°C of 0.0001 MPa or more and 1 MPa or less after being irradiated with ultraviolet light of 100°C for 120 hours.

10. The pressure-sensitive adhesive sheet according to claim 1, wherein the peak temperature of the loss tangent tan δ of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer after lamination is -30°C or higher and 30°C or lower.

11. Illuminance of the adhesive layer after lamination is 100 mW / cm 2 2. The pressure-sensitive adhesive sheet according to claim 1, wherein the pressure-sensitive adhesive layer has a peak temperature of loss tangent tan δ of −30° C. or higher and 30° C. or lower after being irradiated with ultraviolet light of 1000 nm for 120 hours.

12. The adhesive sheet according to any one of claims 1 to 11, characterized in that the adhesive constituting the adhesive layer is an active energy ray-curable adhesive, and the adhesive layer after lamination is an active energy ray-cured adhesive layer.

13. The adhesive sheet according to claim 12, characterized in that the gel fraction of the adhesive constituting the adhesive layer before curing with active energy rays is 20% or more and 85% or less.

14. The adhesive sheet according to claim 1, wherein the adhesive is an acrylic adhesive.

15. The adhesive sheet according to claim 1, characterized in that the adhesive sheet comprises two release sheets, and the adhesive layer is sandwiched between the release sheets so as to be in contact with the release surfaces of the two release sheets.

16. A display comprising: one display component; another display component; and an adhesive layer for bonding said one display component and said other display component to each other, wherein said adhesive layer is formed from an adhesive layer of the adhesive sheet described in claim 1.

17. The display according to claim 16, wherein both the first display member and the second display member are hard plates.

Citation Information

Patent Citations

  • Adhesive sheet and laminate

    JP2015010197A

  • Adhesive sheet, display body and manufacturing method therefor

    JP2017149807A

  • Adhesive sheet and display body

    JP2019035061A

  • Constituent and method for manufacturing the same, display body, and adhesive sheet for optical use

    JP2019042965A

  • Adhesive sheet, display body and method for manufacturing display body

    JP2019044023A

Cited By

  • Adhesive, adhesive sheet, optical structure, and display body

    JPWO2025203862A1