Multilayer structure
The multilayer structure design with strategically placed metal and glass layers and an optimized adhesive peel force addresses the issue of glass layer damage during removal, ensuring safe peeling by reducing the probability of breakage to 50% or less.
Patent Information
- Application Number
- PCT/JP2024/007103
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-02-27
- Publication Date
- 2024-10-03
AI Technical Summary
The existing multilayer structures face the risk of glass layer damage when peeled off from an adherend due to strong adhesive forces, which can lead to breakage during repair or removal processes.
A multilayer structure design featuring a support with a glass layer laminated on top, a metal layer between the support and glass, and another metal layer on the bottom, along with an adhesive layer on the support's lower surface, where the glass layer thickness is between 10 μm and 300 μm, and the adhesive's 45-degree peel force is set to ensure a 50% or less probability of glass breakage in a breakage test.
This configuration reduces the likelihood of glass layer damage during peeling by optimizing the adhesive's peeling force, ensuring the multilayer structure can be safely removed from adherends without glass breakage.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure 00000015_0000 
Figure 00000016_0000
Abstract
Description
Multi-layer structure
[0001] The present invention relates to a multi-layer structure.
[0002] Multilayer structures in which two or more layers are laminated are known. One example is a multilayer structure in which a silver reflective layer is laminated on a thin glass layer (glass film). The thickness of this multilayer structure is, for example, in the range of 10 to 200 μm. This multilayer structure can be obtained, for example, from a glass roll formed by a down-draw method.
[0003] JP 2013-231744 A
[0004] It is also conceivable to use a resin support as the support of a multilayer structure, provide a metal layer on the resin support, and use the multilayer structure as a mirror. This multilayer structure is used by, for example, attaching the support to an adherend such as a wall via an adhesive layer or the like.
[0005] However, if the peel strength (separation strength) of the adhesive layer or the like is strong, there is a risk that the glass layer may be damaged when the multilayer structure is peeled off from the adherend for repair or the like.
[0006] The present invention has been made in view of the above points, and has as its object to make it difficult for the glass layer to break when peeling the multilayer structure from the adherend.
[0007] This multilayer structure comprises a support, a glass layer laminated on the upper surface of the support, a metal layer laminated between the support and the glass layer, and an adhesive portion provided on the lower surface of the support, wherein the thickness of the glass layer is 10 μm or more and 300 μm or less, and the 45-degree peel force of the adhesive portion is set so that the probability of breakage in a glass layer breakage test is 50% or less.
[0008] According to the disclosed technology, the glass layer can be made less susceptible to breakage when the multilayer structure is peeled off from the adherend.
[0009] Fig. 1 is a cross-sectional view illustrating a multilayer structure according to the present embodiment; Fig. 2 is a cross-sectional view illustrating a multilayer structure according to a modified example 1 of the present embodiment; Fig. 3 is a cross-sectional view illustrating a multilayer structure according to a modified example 2 of the present embodiment; Fig. 4 is a view illustrating a method of a glass layer fracture test; Fig. 5 is a view illustrating the results of a glass layer fracture test.
[0010] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The following describes the preferred embodiments of the present invention with reference to the accompanying drawings. In the drawings, the same components are designated by the same reference numerals, and redundant explanations may be omitted.
[0011] Fig. 1 is a cross-sectional view illustrating a multilayer structure according to this embodiment. As shown in Fig. 1, the multilayer structure 1 includes a support 10, a bonding layer 20, a thin glass mirror 30, and an adhesive portion 40. In the multilayer structure 1, the thin glass mirror 30 is laminated on the upper surface 10a of the support 10 via the bonding layer 20. The adhesive portion 40 is provided on the lower surface 10b of the support 10.
[0012] The thin glass mirror 30 has a resin layer 31, a metal layer 32, an adhesive layer 33, and a glass layer 34. However, the resin layer 31 and the adhesive layer 33 can be provided as needed. For example, the thin glass mirror 30 may not have the resin layer 31 or the adhesive layer 33, and the metal layer 32 may be formed directly on the lower surface of the glass layer 34.
[0013] The planar shape of the multilayer structure 1 (the shape when viewed from the normal direction of the upper surface 10a of the support 10) is, for example, rectangular. However, this is not limited thereto, and the planar shape of the multilayer structure 1 can be circular, elliptical, a combination of these, or any other appropriate shape. Furthermore, the planar shapes of each layer do not have to be the same. For example, the planar shape of the support 10 may be larger than the planar shape of the thin glass mirror 30. The multilayer structure 1 can be used, for example, as a mirror.
[0014] Here, the materials of each part of the multi-layer structure 1 will be described.
[0015] [Support] The support 10 supports the thin glass mirror 30. The thickness of the support 10 can be, for example, 0.1 mm or more and 5 mm or less. Materials that can be used for the support 10 include resin, metal, glass, etc. Examples of resin include polycarbonate and polypropylene. Examples of metal include aluminum, stainless steel (SUS), copper, etc. Using a resin support 10 makes it possible to realize a flexible multilayer structure 1. For example, it becomes possible to attach the multilayer structure 1 along a curved surface.
[0016] [Bonding Layer] The bonding layer 20 is laminated on the support 10. As the bonding layer 20, any adhesive or pressure-sensitive adhesive can be used.
[0017] In this specification, a pressure-sensitive adhesive refers to a layer that has adhesive properties at room temperature and adheres to an adherend with light pressure. Therefore, even when an adherend that has been stuck to the pressure-sensitive adhesive is peeled off, the pressure-sensitive adhesive retains practical adhesive strength. On the other hand, an adhesive refers to a layer that can bond substances by being interposed between them. Therefore, when an adherend that has been stuck to the adhesive is peeled off, the adhesive no longer has practical adhesive strength.
[0018] When a pressure-sensitive adhesive is used for the bonding layer 20, a pressure-sensitive adhesive having a base polymer such as an acrylic polymer, a silicone polymer, polyester, polyurethane, polyamide, polyether, a fluorine-based polymer, or a rubber-based polymer is used. When a pressure-sensitive adhesive is used for the bonding layer 20, an acrylic pressure-sensitive adhesive is preferably used. This is because acrylic pressure-sensitive adhesives have excellent optical transparency and exhibit adhesive properties such as appropriate wettability, cohesion, and adhesion, and can have excellent weather resistance, heat resistance, and the like. In particular, an acrylic pressure-sensitive adhesive made of an acrylic polymer having 4 to 12 carbon atoms is preferred.
[0019] When an adhesive is used for the bonding layer 20, for example, a polyester adhesive, a polyurethane adhesive, a polyvinyl alcohol adhesive, or an epoxy adhesive is used. When the adhesive is a thermosetting adhesive, peel resistance can be exerted by heating and curing (solidifying). When the adhesive is a light-curing adhesive such as an ultraviolet-curing adhesive, peel resistance can be exerted by curing it with light such as ultraviolet light. When the adhesive is a moisture-curing adhesive, it can harden by reacting with moisture in the air, and therefore it can harden and exert peel resistance even when left alone.
[0020] [Resin Layer] In the example of FIG. 1 , a resin layer 31 is provided between a metal layer 32 and a glass layer 34. The resin layer 31 can be composed of, for example, one layer or multiple layers. When the resin layer 31 is composed of multiple layers, it is preferable to laminate the layers with an adhesive layer interposed therebetween. From the viewpoint of flexibility, the total thickness of the resin layer 31 may be 20 μm or more and 1000 μm or less, preferably 25 μm or more and 500 μm or less, and more preferably 50 μm or more and 200 μm or less. When the resin layer 31 is composed of a single layer, the thickness of the resin layer 31 can be, for example, 20 μm or more and 150 μm or less.
[0021] Examples of materials for the resin layer 31 include polyester resins such as polyethylene terephthalate resins and polyethylene naphthalate resins, cycloolefin resins such as norbornene resins, polyethersulfone resins, polycarbonate resins, acrylic resins, polyolefin resins, polyimide resins, polyamide resins, polyimideamide resins, polyarylate resins, polysulfone resins, polyetherimide resins, cellulose resins, and urethane resins.
[0022] The resin layer 31 is provided as needed, but providing the resin layer 31 has the effect of improving the handling properties of the multilayer structure 1 .
[0023] [Metal Layer] The metal layer 32 is laminated between the support 10 and the glass layer 34. In the example of FIG. 1, the metal layer 32 is laminated on the lower surface of the resin layer 31. In addition, in the example of FIG. 1, the side of the metal layer 32 opposite to the resin layer 31 is bonded to the support 10 via a bonding layer 20. The metal layer 32 is a layer that reflects visible light incident through the glass layer 34. In other words, the upper surface 32a of the metal layer 32 (the surface in contact with the resin layer 31) is a reflective surface that reflects visible light incident through the glass layer 34. Note that in the example of FIG. 1, visible light is incident on the upper surface 32a of the metal layer 32 via the glass layer 34, the adhesive layer 33, and the resin layer 31.
[0024] The metal layer 32 may be laminated between the support 10 and the glass layer 34, and is not limited to the example shown in FIG. 1 . The metal layer 32 may be laminated on, for example, the resin layer 31. For example, as in the multilayer structure 1A shown in FIG. 2 , a structure in which a bonding layer 20, a resin layer 31, a metal layer 32, an adhesive layer 33, and a glass layer 34 are laminated in this order on the upper surface 10 a of the support 10 may be used. The metal layer 32 can be formed on the upper surface of the resin layer 31 by, for example, a sputtering method, a vapor deposition method, a plating method, or the like.
[0025] Alternatively, the metal layer 32 may be formed on the lower surface of the glass layer 34. For example, as in the multilayer structure 1B shown in Fig. 3 , a structure can be used in which a bonding layer 20, a resin layer 31, an adhesive layer 33, a metal layer 32, and a glass layer 34 are sequentially stacked on the upper surface 10a of the support body 10. The metal layer 32 can be formed on the lower surface of the glass layer 34 by, for example, a sputtering method, a vapor deposition method, a plating method, or the like.
[0026] In the multilayer structure 1 shown in Figure 1, the metal layer 32 is located below the resin layer 31, which makes it possible to reduce scratches that occur during the process. That is, when manufacturing a multilayer structure, if an adhesive that becomes the adhesive layer 33 is applied to the surface of the metal layer 32 and spread thinly, the surface of the metal layer 32 is easily scratched when spreading thinly. The structure in Figure 1 does not require the step of applying and spreading an adhesive to the surface of the metal layer 32, so scratches on the surface of the metal layer 32 can be suppressed.
[0027] 2, the metal layer 32 is located above the resin layer 31, so that the reflected light is not affected by the light absorption of the resin layer 31, and therefore clearer reflection characteristics can be obtained. Also, in the multilayer structure 1B shown in FIG. 3, the metal layer 32 is located directly below the glass layer 34, so that the reflected light is not affected by the light absorption of the resin layer 31 or the adhesive layer 33, and therefore clearer reflection characteristics can be obtained.
[0028] The material of the metal layer 32 is preferably a material with high visible light reflectance, such as aluminum, silver, or a silver alloy. The visible light reflectance of the metal layer 32 alone is preferably 70% or more, more preferably 75% or more, and even more preferably 83% or more. The visible light reflectance of the metal layer 32 alone can be measured by a method in accordance with JIS R3220:2011.
[0029] The thickness of the metal layer 32 is not particularly limited, but is, for example, approximately 10 nm to 500 nm. The metal layer 32 can be formed directly on the lower surface of the resin layer 31 by, for example, sputtering, vapor deposition, plating, etc. When the resin layer 31 is not provided, the metal layer 32 may be formed on the lower surface of the glass layer 34 by, for example, sputtering, vapor deposition, plating, etc. Alternatively, the metal layer 32 may be formed on the upper surface 10 a of the support 10 by, for example, sputtering, vapor deposition, plating, etc.
[0030] [Adhesive Layer] The adhesive layer 33 is formed from a material with high visible light transmittance. The thickness of the adhesive layer 33 is, for example, 0.1 μm or more and 25 μm or less. For example, the adhesive layer 33 can be made of an acrylic adhesive, a silicone adhesive, a rubber adhesive, a UV-curable acrylic adhesive, a UV-curable epoxy adhesive, a thermosetting epoxy adhesive, a thermosetting melamine adhesive, a thermosetting phenol adhesive, an ethylene vinyl acetate (EVA) interlayer, or a polyvinyl butyral (PVB) interlayer.
[0031] [Glass Layer] The glass layer 34 is laminated on the upper surface 10a side of the support 10. In the example of FIG. 1, the glass layer 34 is laminated on the resin layer 31 via an adhesive layer 33. There are no particular limitations on the glass layer 34, and an appropriate glass layer can be adopted depending on the purpose. The glass layer 34 can be classified by composition, for example, soda-lime glass, borate glass, aluminosilicate glass, quartz glass, etc. Furthermore, the glass layer 34 can be classified by alkali component, for example, alkali-free glass or low-alkali glass. The alkali metal component (e.g., Na) of the glass can be 2 O.K. 2 O, Li 2 The content of O) is preferably 15% by weight or less, more preferably 10% by weight or less.
[0032] Considering the surface hardness, airtightness, and corrosion resistance of glass, the thickness of the glass layer 34 is preferably 10 μm or more. Furthermore, since it is desirable for the glass layer 34 to have flexibility like a film, the thickness of the glass layer 34 is preferably 300 μm or less. The thickness of the glass layer 34 is more preferably 20 μm or more and 200 μm or less, and particularly preferably 30 μm or more and 150 μm or less.
[0033] The glass layer 34 preferably has a light transmittance of 85% or more at a wavelength of 550 nm. The glass layer 34 preferably has a refractive index of 1.4 to 1.65 at a wavelength of 550 nm. The glass layer 34 preferably has a density of 2.3 g / cm 3 ~3.0 g / cm 3 and more preferably 2.3 g / cm 3 ~2.7g / cm 3 is.
[0034] The method for forming the glass layer 34 is not particularly limited, and an appropriate method can be adopted depending on the purpose. Typically, the glass layer 34 can be produced by melting a mixture containing a main raw material such as silica or alumina, an antifoaming agent such as mirabilite or antimony oxide, and a reducing agent such as carbon at a temperature of approximately 1400°C to 1600°C, forming it into a thin plate, and then cooling it. Examples of methods for forming the glass layer 34 include the slot downdraw method, the fusion method, and the float method. The glass layer formed into a plate shape by these methods may be chemically polished with a solvent such as hydrofluoric acid, as necessary, to make it thinner or to improve smoothness.
[0035] In addition, a functional layer such as an antifouling layer, an anti-reflection layer, a conductive layer, a reflective layer, or a decorative layer may be provided on the upper surface of the glass layer 34 (the surface on which the adhesive layer 33 is not formed).
[0036] [Adhesive portion 40] The adhesive portion 40 is used to attach the multilayer structure 1 to the adherend. Considering rework, the adhesive portion 40 is preferably one that allows the multilayer structure 1 to be easily peeled from the adherend. Here, rework refers to, for example, a case where an attachment error occurs during construction and the multilayer structure is reattached. In such a case, if the peel strength of the adhesive portion 40 is too strong, the glass layer 34 of the thin glass mirror 30 may be damaged when the multilayer structure 1 is peeled from the adherend. On the other hand, by appropriately setting the peel strength of the adhesive portion 40, the risk of damage to the glass layer 34 of the thin glass mirror 30 when the multilayer structure 1 is peeled from the adherend can be reduced.
[0037] The adhesive portion 40 can be formed using any of the materials exemplified as the adhesive for the bonding layer 20, as long as it has an appropriate peel strength. Alternatively, the adhesive portion 40 may be a double-sided tape, a hook-and-loop fastener, or the like, as long as it has an appropriate peel strength. The thickness of the adhesive portion 40 is not particularly limited, but is, for example, about 5 μm or more and 2000 μm or less.
[0038] [Study on Peel Strength of Adhesive Portion 40] The multilayer structure 1 is attached to an adherend via the adhesive portion 40. The adherend is typically a building material such as a wall containing calcium silicate. Alternatively, the adherend may be a material generally used in building applications, such as gypsum board, wallpaper, wood, metal, or glass.
[0039] Conventionally, an adhesive with strong peel strength has been used for the adhesive portion 40. Therefore, the adhesive portion 40 adheres closely to the adherend, and a large force is required to peel it off, which may cause damage to the glass layer 34 of the thin glass mirror 30 when peeling the multilayer structure 1 from the adherend.
[0040] Therefore, the inventors investigated the peel strength of the adhesive portion 40 that allows the multilayer structure 1 to be peeled off from the adherend without damaging the glass layer 34. Specifically, the following glass layer destruction test was carried out in an environment of room temperature (25°C).
[0041] 4 is a diagram illustrating the method of the glass layer destruction test. First, 10 pieces each of a hook-and-loop fastener, double-sided tape A, and double-sided tape B were prepared as adhesive portions 40. Double-sided tapes A and B are conventionally used double-sided tapes and have relatively strong peel strength.
[0042] Next, 40 multilayer structures 1 shown in FIG. 4 were produced using 10 of each adhesive portion 40. The planar shape of the multilayer structure 1 was 20 mm × 220 mm. A polycarbonate sheet having a thickness of 0.4 mm was used as the support 10. The metal layer 32 was an aluminum film having a thickness of 50 nm. The thickness of the glass layer 34 was 100 μm.
[0043] Next, an adherend 100 having a thickness of 1.3 mm was prepared, and the adhesive portion 40 of the multilayer structure 1 was attached to the flat upper surface 100a of the adherend 100. Plate glass was used as the adherend 100. An end of the adherend 100 was fixed to the fixing portion 120 via a string 110. The angle θ between the upper surface 100a of the adherend 100 and the upper surface 120a of the fixing portion 120 was 45 degrees.
[0044] Next, the adherend 100 was moved at 300 mm / min in a direction A perpendicular to the upper surface 100a, the adhesive portion 40 was peeled off from the upper surface 100a of the adherend 100, and the 45-degree peel force (N / 20 mm) was measured. After peeling, the glass layer 34 was visually inspected for damage. Specifically, if even one crack penetrated the glass layer 34, it was determined that damage had occurred.
[0045] The same test was performed on all 40 multilayer structures 1 to determine the 45-degree peel force and the probability of failure. The average values of the 45-degree peel force and the probability of failure of the four types of adhesive portion 40 are summarized in Table 1. The probability of failure is the ratio of the number of multilayer structures in which the glass layer was broken to the number of multilayer structures tested.
[0046]
[0047] As shown in Table 1, when the adhesive portion 40 was a hook-and-loop fastener, the 45-degree peel force was 7.5 (N / 20 mm) and the failure probability was 20%.
[0048] In contrast, when the adhesive portion 40 was double-sided tape A, the 45-degree peel force was 68.2 (N / 20 mm) and the failure probability was 100%. When the adhesive portion 40 was double-sided tape B, the 45-degree peel force was 38.5 (N / 20 mm) and the failure probability was 80%.
[0049] In this way, by using a hook-and-loop fastener as the adhesive portion 40, it was found that it was possible to reduce the 45-degree peel force compared to the double-sided tapes A and B that were previously used, and the probability of breakage could be significantly reduced.
[0050] Next, the results of Table 1 were summarized in Figure 5, and the approximate formula y = 1.4895x + 7.4351 was calculated. In Figure 5, the horizontal axis (x) represents the 45-degree peel force (N / 20 mm), and the vertical axis (y) represents the failure probability (%). Since the failure probability of the conventionally used double-sided tapes A and B is 80% to 100%, it was determined that a failure probability of 50% or less (y = 50 or less) would be a sufficient improvement, and the pass mark was set to be a failure probability of 50% or less.
[0051] 5, from the viewpoint of further suppressing breakage of the thin glass mirror 30, it is preferable to satisfy the range of 0.03≦x≦28.57, where y = 1.4895x + 7.4351. Here, x = 0.03 (N / 20 mm) is the minimum 45-degree peel force required when attaching the multilayer structure 1 to an adherend. Also, x = 28.57 (N / 20 mm) is the 45-degree peel force at which y = 50 (%) in the above approximation formula.
[0052] Thus, in the multilayer structure 1, the adhesive portion 40 is preferably set at a 45-degree peel force so that the fracture probability in a glass layer fracture test is 50% or less. Furthermore, it is more preferable that the adhesive portion 40 has a 45-degree peel force set so that the fracture probability in a glass layer fracture test is 20% or less. Furthermore, when x is the 45-degree peel force (N / 20 mm) and y is the fracture probability (%), it is even more preferable that the range of 0.03≦x≦28.57, where y = 1.4895x + 7.4351, is satisfied. This makes it possible to make the glass layer 34 of the thin glass mirror 30 less likely to break when the multilayer structure 1 is peeled off from the adherend.
[0053] In the above, a hook-and-loop fastener is exemplified as the adhesive portion 40 for which the 45-degree peel force can be set so that the probability of failure in the glass layer failure test is 50% or less. However, the present invention is not limited to this, and other materials or adhesives may be used as long as the 45-degree peel force can be set so that the probability of failure in the glass layer failure test is 50% or less.
[0054] The above describes preferred embodiments in detail, but the present invention is not limited to the above-described embodiments, and various modifications and substitutions can be made to the above-described embodiments without departing from the scope of the claims.
[0055] In addition to the above embodiments, the following supplementary notes are further disclosed. (Supplementary Note 1) A multilayer structure comprising: a support; a glass layer laminated on an upper surface of the support; a metal layer laminated between the support and the glass layer; and an adhesive portion provided on a lower surface of the support, wherein the thickness of the glass layer is 10 μm or more and 300 μm or less, and the adhesive portion has a 45-degree peel force set so that the probability of failure in a glass layer failure test is 50% or less. (Supplementary Note 2) The multilayer structure according to Supplementary Note 1, wherein the 45-degree peel force of the adhesive portion is set so that the probability of failure in a glass layer failure test is 20% or less. (Supplementary Note 3) The multilayer structure according to Supplementary Note 1 or 2, wherein, when x is the 45-degree peel force (N / 20 mm) and y is the probability of failure (%), the range of 0.03≦x≦28.57, where y = 1.4895x + 7.4351, is satisfied. (Appendix 4) The multilayer structure according to any one of Appendices 1 to 3, wherein the adhesive portion is a hook-and-loop fastener. (Appendix 5) The multilayer structure according to any one of Appendices 1 to 4, wherein a resin layer is provided between the metal layer and the glass layer. (Appendix 6) The multilayer structure according to Appendices 5, wherein the glass layer is laminated on an upper surface side of the resin layer via an adhesive layer, the metal layer is laminated on a lower surface of the resin layer, and the side of the metal layer opposite to the resin layer is joined to the support via a joining layer.
[0056] This international application claims priority based on Japanese Patent Application No. 2023-050362, filed on March 27, 2023, the entire contents of which are incorporated herein by reference.
[0057] REFERENCE SIGNS LIST 1, 1A, 1B Multilayer structure 10 Support 10a Upper surface 10b Lower surface 20 Bonding layer 30 Thin glass mirror 31 Resin layer 32 Metal layer 33 Adhesive layer 34 Glass layer 40 Adhesive portion
Claims
1. A multilayer structure comprising: a support; a glass layer laminated on an upper surface of the support; a metal layer laminated between the support and the glass layer; and an adhesive portion provided on a lower surface of the support, wherein the thickness of the glass layer is 10 μm or more and 300 μm or less, and the adhesive portion has a 45 degree peel force set so that the probability of failure in a glass layer failure test is 50% or less.
2. The multi-layer structure according to claim 1, wherein the adhesive portion has a 45-degree peel force set so that the probability of breakage in a glass layer breakage test is 20% or less.
3. The multi-layer structure according to claim 1, which satisfies the range of 0.03≦x≦28.57 of y=1.4895x+7.4351, where x is a 45-degree peel force (N / 20 mm) and y is a fracture probability (%).
4. The multi-layer structure according to any one of claims 1 to 3, wherein the adhesive portion is a hook-and-loop fastener.
5. The multi-layer structure according to any one of claims 1 to 3, further comprising a resin layer provided between the metal layer and the glass layer.
6. The multi-layer structure according to claim 5, wherein the glass layer is laminated on the upper surface side of the resin layer via an adhesive layer, the metal layer is laminated on the lower surface of the resin layer, and the side of the metal layer opposite the resin layer is joined to the support via a joining layer.
Citation Information
Patent Citations
Multilayer structure
WO2021199985A1
Multilayer structure
WO2021199986A1
Multi-layer structure
WO2022113652A1