Resin composition, prepreg, film with resin, metal foil with resin, metal-clad laminate, and wiring board

WO2024202879A1PCT designated stage expired Publication Date: 2024-10-03PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/007426
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-02-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Wiring boards in electronic devices face challenges with warping of semiconductor packages due to thermal expansion issues and require materials with low coefficient of thermal expansion and high plating adhesion to maintain mechanical integrity and signal transmission efficiency.

Method used

A resin composition comprising a maleimide compound with an indane structure, a benzoxazine compound with an allyl group, and a styrenic polymer, which, when cured, provides a low coefficient of thermal expansion and high plating adhesion, suitable for use in prepregs, metal-clad laminates, and wiring boards.

Benefits of technology

The resin composition effectively suppresses thermal expansion and ensures strong adhesion, enhancing the mechanical and electrical performance of wiring boards by maintaining signal integrity and preventing delamination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024007426_03102024_PF_FP_ABST
    Figure JP2024007426_03102024_PF_FP_ABST
Patent Text Reader

Abstract

One aspect of the present invention provides a resin composition which contains a maleimide compound (A) that has an indane structure represented by formula (1) in each molecule, a benzoxazine compound (B) that has an allyl group in each molecule, and a styrene polymer (C) that is in a solid state at 25°C. In formula (1), each Rb independently represents an alkyl group having 1 to 10 carbon atoms, an alkyloxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a nitro group, a hydroxyl group or a mercapto group; and r represents 0 to 3.
Need to check novelty before this filing date? Find Prior Art

Description

Resin composition, prepreg, resin-coated film, resin-coated metal foil, metal-clad laminate, and wiring board

[0001] The present invention relates to a resin composition, a prepreg, a resin-coated film, a resin-coated metal foil, a metal-clad laminate, and a wiring board.

[0002] As the amount of information processed in various electronic devices increases, packaging technologies such as higher integration, higher wiring density, and multi-layering of the semiconductor devices mounted thereon are advancing. Furthermore, wiring boards used in various electronic devices are required to be high-frequency compatible, such as millimeter-wave radar substrates for automotive applications. Substrate materials for constituting the insulating layers of wiring boards used in various electronic devices are required to have low relative dielectric constants and dielectric loss tangents in order to increase signal transmission speeds and reduce signal transmission losses. Examples of substrate materials with low relative dielectric constants and dielectric loss tangents include resin compositions described in Patent Documents 1 and 2.

[0003] Patent Document 1 describes a resin composition containing a maleimide compound, an allyl group-containing benzoxazine compound, and a high-molecular-weight component. Patent Document 1 discloses that it is possible to provide a resin composition that has a small dielectric loss tangent value, excellent adhesion to conductive materials after environmental resistance testing, and is capable of producing a cured product with improved brittleness.

[0004] Patent Document 2 describes a resin composition containing a maleimide compound having an indane structure in the molecule and a styrene-based polymer that is solid at 25° C. Patent Document 2 discloses that it is possible to provide a resin composition that has low dielectric properties, excellent adhesion to metal foil, a high glass transition temperature, and that can give a cured product in which increases in relative dielectric constant and dielectric loss tangent due to temperature are sufficiently suppressed.

[0005] Metal-clad laminates and resin-coated metal foils used in manufacturing wiring boards and the like have not only an insulating layer but also a metal foil on the insulating layer. Similarly, wiring boards also have not only an insulating layer but also wiring on the insulating layer. Examples of the wiring include wiring derived from the metal foil provided on the metal-clad laminates and the like.

[0006] In recent years, small portable devices, such as mobile communication terminals and notebook PCs, have rapidly become more multifunctional, high-performance, thin, and compact. Accordingly, wiring boards used in these products are also required to have finer conductor wiring, more multilayered conductor wiring layers, thinner designs, and higher performance in terms of mechanical properties. In particular, as wiring boards become thinner, warping occurs in semiconductor packages mounting semiconductor chips on the wiring board, which increases the likelihood of mounting defects. To suppress warping in semiconductor packages mounting semiconductor chips on wiring boards, the insulating layer is required to have a low thermal expansion coefficient (thermal expansion rate). Therefore, substrate materials for constituting the insulating layer of wiring boards are required to produce cured products with a low thermal expansion coefficient.

[0007] In the manufacture of wiring boards, for example, when forming multiple conductor wiring layers, holes are drilled in the insulating layer using a drill such as a mechanical drill and a laser such as a carbon dioxide laser to connect the individual conductor wiring layers, and then a desmear process is performed to clean the holes formed by the drilling process, followed by electrolytic plating processes such as electroless plating and electrolytic copper plating. Conductive wiring formed by such electroless plating and electrolytic plating processes is required to be resistant to peeling from the insulating layer. Therefore, substrate materials for forming the insulating layers of wiring boards are required to produce cured products with high plating adhesion.

[0008] For these reasons, substrate materials for forming insulating layers of wiring boards are required to have a low thermal expansion coefficient and to provide a cured product with high plating adhesion.

[0009] JP 2020-158705 A International Publication No. 2022 / 054864

[0010] The present invention has been made in view of the above circumstances, and aims to provide a resin composition that can give a cured product having a low thermal expansion coefficient and high plating adhesion. It is also an object of the present invention to provide a prepreg, a resin-coated film, a resin-coated metal foil, a metal-clad laminate, and a wiring board that can be obtained using the resin composition.

[0011] One aspect of the present invention is a resin composition containing a maleimide compound (A) having an indane structure represented by the following formula (1) in the molecule, a benzoxazine compound (B) having an allyl group in the molecule, and a styrene-based polymer (C) that is solid at 25°C:

[0012] In formula (1), each Rb independently represents an alkyl group having 1 to 10 carbon atoms, an alkyloxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a nitro group, a hydroxyl group, or a mercapto group; and r represents an integer of 0 to 3.

[0013] These and other objects, features, and advantages of the present invention will become apparent from the following detailed description and the accompanying drawings.

[0014] Fig. 1 is a schematic cross-sectional view showing an example of a prepreg according to an embodiment of the present invention. Fig. 2 is a schematic cross-sectional view showing an example of a metal-clad laminate according to an embodiment of the present invention. Fig. 3 is a schematic cross-sectional view showing an example of a wiring board according to an embodiment of the present invention. Fig. 4 is a schematic cross-sectional view showing an example of a resin-coated metal foil according to an embodiment of the present invention. Fig. 5 is a schematic cross-sectional view showing an example of a resin-coated film according to an embodiment of the present invention.

[0015] As a result of extensive investigations, the present inventors have found that the above object can be achieved by the present invention described below.

[0016] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these.

[0017] [Resin Composition] A resin composition according to one embodiment of the present invention is a resin composition containing a maleimide compound (A) having an indane structure represented by the following formula (1) in the molecule, a benzoxazine compound (B) having an allyl group in the molecule, and a styrene-based polymer (C) that is solid at 25° C. By curing the resin composition, a cured product having a low thermal expansion coefficient and high plating adhesion can be obtained.

[0018] (Maleimide Compound (A)) The maleimide compound (A) is not particularly limited as long as it is a maleimide compound having an indane structure represented by the formula (1) in the molecule. The maleimide compound (A) has not only the indane structure but also a maleimide group in the molecule. Specific examples of the maleimide compound (A) include maleimide compounds (A1) having a structure represented by the following formula (2) in the molecule.

[0019] In formula (1), each Rb is independent. That is, each Rb may be the same group or different groups. For example, when r is 2 or 3, two or three Rb's bonded to the same benzene ring may be the same group or different groups. Rb represents an alkyl group having 1 to 10 carbon atoms, an alkyloxy group (alkoxy group) having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a nitro group, a hydroxyl group, or a mercapto group (thiol group). r represents an integer of 0 to 3.

[0020] In formula (2), each Ra is independent. That is, each Ra may be the same group or different groups. For example, when q is 2 to 4, 2 to 4 Ra bonded to the same benzene ring may be the same group or different groups. Ra represents an alkyl group having 1 to 10 carbon atoms, an alkyloxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a nitro group, a hydroxyl group, or a mercapto group. Rb's are the same as Rb's in formula (1), and each independently represents an alkyl group having 1 to 10 carbon atoms, an alkyloxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a nitro group, a hydroxyl group, or a mercapto group. q represents 0 to 4. r represents 0 to 3. n represents 0.95 to 10.

[0021] r is the average value of the degree of substitution of Rb, and a smaller value is preferable, specifically 0. That is, in the benzene ring to which Rb can be bonded, a hydrogen atom is preferably bonded at the position to which Rb can be bonded. The maleimide compound (A) having such an r is easy to synthesize. This is thought to be due to reduced steric hindrance and increased electron density in the aromatic ring. Furthermore, when r is 1 to 3, Rb is preferably at least one selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, and an aryl group having 6 to 10 carbon atoms. Furthermore, Ra is preferably at least one selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, and an aryl group having 6 to 10 carbon atoms. The alkyl group having 1 to 4 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, and an aryl group having 6 to 10 carbon atoms improves solubility in solvents and suppresses a decrease in the reactivity of the maleimide group, resulting in a suitable cured product. This is thought to be due to a decrease in planarity in the vicinity of the maleimide group, a decrease in crystallinity, and the like.

[0022] Specific examples of the groups represented by Ra and Rb include the following groups.

[0023] The alkyl group having 1 to 10 carbon atoms is not particularly limited, and examples thereof include a methyl group, an ethyl group, a propyl group, a hexyl group, and a decyl group.

[0024] The alkyloxy group having 1 to 10 carbon atoms is not particularly limited, and examples thereof include a methyloxy group, an ethyloxy group, a propyloxy group, a hexyloxy group, and a decyloxy group.

[0025] The alkylthio group having 1 to 10 carbon atoms is not particularly limited, and examples thereof include a methylthio group, an ethylthio group, a propylthio group, a hexylthio group, and a decylthio group.

[0026] The aryl group having 6 to 10 carbon atoms is not particularly limited, and examples thereof include a phenyl group and a naphthyl group.

[0027] The aryloxy group having 6 to 10 carbon atoms is not particularly limited, and examples thereof include a phenyloxy group and a naphthyloxy group.

[0028] The arylthio group having 6 to 10 carbon atoms is not particularly limited, and examples thereof include a phenylthio group and a naphthylthio group.

[0029] The cycloalkyl group having 3 to 10 carbon atoms is not particularly limited, and examples thereof include a cyclopropyl group, a cyclobutyl group, a cyclohexyl group, and a cyclooctyl group.

[0030] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.

[0031] q is the average value of the substitution degree of Ra, and is preferably 2 to 3, and more preferably 2. The maleimide compound (A) having such a q is easy to synthesize. This is thought to be because, particularly when q is 2, steric hindrance is reduced and the electron density of the aromatic ring is increased.

[0032] n is the average number of repeats, and as described above, is 0.95 to 10, preferably 0.98 to 8, more preferably 1 to 7, and even more preferably 1.1 to 6. In the maleimide compound represented by formula (1) and the maleimide compound (A1) represented by formula (2), the content of the maleimide compound in which n, the average number of repeats (degree of polymerization), is 0, is preferably 32 mass% or less based on the total amount of the maleimide compound (A).

[0033] The maleimide compound (A) preferably has a molecular weight distribution (Mw / Mn) measured by gel permeation chromatography (GPC) of 1 to 4, more preferably 1.1 to 3.8, even more preferably 1.2 to 3.6, and particularly preferably 1.3 to 3.4. The molecular weight distribution is measured by gel permeation chromatography (GPC).

[0034] The maleimide compound (A) may not only have the indane structure represented by formula (1) in the molecule, but may also have an arylene structure in the molecule that is oriented and bonded at the meta position. That is, examples of the maleimide compound (A) include maleimide compounds having the indane structure and the arylene structure in the molecule. Examples of the arylene structure oriented and bonded at the meta position include an arylene structure in which a structure containing a maleimide group (i.e., other than Rb) is bonded at the meta position (an arylene structure in which a structure containing a maleimide group is substituted at the meta position). The arylene structure oriented and bonded at the meta position is an arylene group oriented and bonded at the meta position, such as a group represented by formula (6) below. Examples of the arylene structure oriented and bonded at the meta position include m-arylene groups such as an m-phenylene group and an m-naphthylene group, and more specifically, a group represented by formula (6) below:

[0035] Specific examples of the maleimide compound (A) include maleimide compounds represented by formulas (7) to (9). These maleimide compounds (A) further have an arylene group in the molecule that is oriented and bonded at the meta position, such as the group represented by formula (6) below.

[0036] In formula (7), n represents 0.95 to 10.

[0037] In formula (8), n represents 0.95 to 10.

[0038] In formula (9), n represents 0.95 to 10.

[0039] The method for producing the maleimide compound (A) is not particularly limited as long as it can produce the maleimide compound (A). Specifically, the maleimide compound (A) can be obtained by a so-called maleimide reaction in which an amine compound represented by the following formula (10) is reacted with maleic anhydride in an organic solvent such as toluene in the presence of a catalyst such as toluenesulfonic acid. More specifically, after the maleimide reaction, unreacted maleic anhydride and other impurities are removed by washing with water or the like, and the solvent is removed under reduced pressure. A dehydrating agent may be used during this reaction. Commercially available products may also be used as the maleimide compound (A).

[0040] In formula (10), each Ra is independent. That is, each Ra may be the same group or different groups. For example, when q is 2 to 4, 2 to 4 Ra bonded to the same benzene ring may be the same group or different groups. Ra represents an alkyl group having 1 to 10 carbon atoms, an alkyloxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a nitro group, a hydroxyl group, or a mercapto group. Rb's are the same as Rb's in formula (1), and each independently represents an alkyl group having 1 to 10 carbon atoms, an alkyloxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a nitro group, a hydroxyl group, or a mercapto group. q represents 0 to 4. r represents 0 to 3. n represents 0.95 to 10.

[0041] The amine compound represented by the formula (10) can be obtained, for example, by reacting 2,6-dimethylaniline with α,α'-dihydroxy-1,3-diisopropylbenzene in an organic solvent such as xylene using activated clay as a catalyst.

[0042] (Benzoxazine Compound (B)) The benzoxazine compound (B) is not particularly limited as long as it is a benzoxazine compound having an allyl group in the molecule. The benzoxazine compound (B) has not only the allyl group but also a benzoxazine group in the molecule. Examples of the benzoxazine group include a benzoxazine group represented by the following formula (3) and a benzoxazine group represented by the following formula (4). Examples of the benzoxazine compound (B) include a benzoxazine compound (B1) having a benzoxazine group represented by the following formula (3) in the molecule, a benzoxazine compound (B2) having a benzoxazine group represented by the following formula (4) in the molecule, and a benzoxazine compound (B3) having a benzoxazine group represented by the following formula (3) and a benzoxazine group represented by the following formula (4) in the molecule.

[0043] In formula (3), R 1 represents an allyl group, and p represents 1 to 4. p represents R 1 is an average value of the degree of substitution of 1 to 4, and is preferably 1.

[0044] In formula (4), R 2 indicates an allyl group.

[0045] Specific examples of the benzoxazine compound (B1) include the benzoxazine compound (B4) represented by the following formula (5), and it is preferable to contain this benzoxazine compound (B4).

[0046] In formula (5), R 3 and R 4 represents an allyl group; X represents an ether bond (—O—) or an alkylene group; q and r each independently represent an integer of 1 to 4.

[0047] The alkylene group is not particularly limited and examples thereof include a methylene group, an ethylene group, a propylene group, a butylene group, a pentylene group, a hexylene group, a heptylene group, an octane group, an icosane group, and a hexatriacontane group. Among these, a methylene group is preferred.

[0048] q is R 3 is the average value of the degree of substitution of R 4 is an average value of the degree of substitution of 1 to 4, and is preferably 1.

[0049] As the benzoxazine compound (B), a commercially available product may be used, for example, ALPd manufactured by Shikoku Chemicals Corporation.

[0050] As the benzoxazine compound (B), the benzoxazine compounds exemplified above may be used alone or in combination of two or more. For example, as the benzoxazine compound (B), the benzoxazine compound (B1) having a benzoxazine group represented by the formula (3) in the molecule, the benzoxazine compound (B2) having a benzoxazine group represented by the formula (4) in the molecule, and the benzoxazine compound (B3) having a benzoxazine group represented by the formula (3) and a benzoxazine group represented by the formula (4) in the molecule may be used alone or in combination of two or more.

[0051] (Styrene-based polymer (C)) The styrene-based polymer (C) is not particularly limited as long as it is a styrene-based polymer that is solid at 25°C. Examples of the styrene-based polymer (C) include styrene-based polymers that are solid at 25°C and can be used as a resin contained in a resin composition used to form an insulating layer provided in a metal-clad laminate, a wiring board, etc. The resin composition used to form an insulating layer provided in a metal-clad laminate, a wiring board, etc. may be a resin composition used to form a resin layer provided in a resin-coated film, a resin-coated metal foil, etc., or may be a resin composition contained in a prepreg.

[0052] The styrene-based polymer (C) may be, for example, a polymer obtained by polymerizing a monomer containing a styrene-based monomer, and may be a styrene-based copolymer. Examples of the styrene-based copolymer include copolymers obtained by copolymerizing one or more of the styrene-based monomers with one or more other monomers copolymerizable with the styrene-based monomer. The styrene-based copolymer may be a random copolymer or a block copolymer, as long as it has a structure derived from the styrene-based monomer in its molecule. Examples of the block copolymer include a binary copolymer of a structure (repeating unit) derived from the styrene-based monomer and the other copolymerizable monomer (repeating unit), and a terpolymer of a structure (repeating unit) derived from the styrene-based monomer, the other copolymerizable monomer (repeating unit), and a structure (repeating unit) derived from the styrene-based monomer. The styrene-based polymer (C) may be a hydrogenated styrene-based copolymer obtained by hydrogenating the styrene-based copolymer. It is preferable that the styrene-based polymer (C) is at least partially hydrogenated. By including an at least partially hydrogenated styrene-based polymer, it is possible to obtain a resin composition which has a low dielectric loss tangent and a low coefficient of thermal expansion and which forms a cured product having excellent toughness.

[0053] The styrene-based monomer is not particularly limited, but examples thereof include styrene, styrene derivatives, styrene in which some of the hydrogen atoms on the benzene ring have been substituted with alkyl groups, styrene in which some of the hydrogen atoms on the vinyl group have been substituted with alkyl groups, vinyltoluene, α-methylstyrene, butylstyrene, dimethylstyrene, and isopropenyltoluene. These styrene-based monomers may be used alone or in combination of two or more. Furthermore, the copolymerizable other monomer is not particularly limited, but examples thereof include olefins such as α-pinene, β-pinene, and dipentene, non-conjugated dienes such as 1,4-hexadiene and 3-methyl-1,4-hexadiene, and conjugated dienes such as 1,3-butadiene and 2-methyl-1,3-butadiene (isoprene). These copolymerizable other monomers may be used alone or in combination of two or more.

[0054] As the styrene-based polymer (C), a wide variety of conventionally known polymers can be used, and there is no particular limitation. For example, a polymer having a structural unit represented by the following formula (11) (a structure derived from the styrene-based monomer) in the molecule can be used.

[0055] In formula (11), R 5 ~R 7 each independently represents a hydrogen atom or an alkyl group, and R 8 represents any group selected from the group consisting of a hydrogen atom, an alkyl group, an alkenyl group, and an isopropenyl group. The alkyl group is not particularly limited, and is preferably, for example, an alkyl group having 1 to 18 carbon atoms, and more preferably an alkyl group having 1 to 10 carbon atoms. Specific examples include a methyl group, an ethyl group, a propyl group, a hexyl group, and a decyl group. The alkenyl group is preferably an alkenyl group having 1 to 10 carbon atoms.

[0056] The styrene-based polymer (C) preferably contains at least one structural unit represented by the formula (11), and may contain a combination of two or more different structural units represented by the formula (11). The styrene-based polymer (C) may also contain a combination of a structural unit represented by the formula (11) and a structural unit other than the structural unit represented by the formula (11). The styrene-based polymer (C) may also contain a structure in which the structural unit represented by the formula (11) is repeated.

[0057] The styrene-based polymer (C) may have, in addition to the structural unit represented by formula (11), at least one of structural units represented by formula (12), formula (13), and formula (14) below, and structures in which the structural units represented by formula (12), formula (13), and formula (14) below are repeated, as structural units derived from other monomers copolymerizable with the styrene-based monomer:

[0058]

[0059]

[0060] In the formula (12), the formula (13) and the formula (14), R 9 ~R 26 are each independently a group selected from the group consisting of a hydrogen atom, an alkyl group, an alkenyl group, and an isopropenyl group. The alkyl group is not particularly limited, and is preferably, for example, an alkyl group having 1 to 18 carbon atoms, and more preferably, an alkyl group having 1 to 10 carbon atoms. Specific examples include a methyl group, an ethyl group, a propyl group, a hexyl group, and a decyl group. The alkenyl group is preferably an alkenyl group having 1 to 10 carbon atoms.

[0061] The styrene-based polymer (C) preferably contains at least one structural unit represented by the formula (12), the formula (13), or the formula (14), and may contain two or more different structural units in combination. The styrene-based polymer may also have at least one structure in which the structural units represented by the formula (12), the formula (13), or the formula (14) are repeated.

[0062] More specifically, examples of the structural unit represented by formula (11) include structural units represented by the following formulas (15) to (17). The structural unit represented by formula (11) may also be a structure in which the structural units represented by formulas (15) to (17) below are respectively repeated. The structural unit represented by formula (11) may be one of these alone or a combination of two or more different types.

[0063]

[0064]

[0065] More specifically, examples of the structural unit represented by formula (12) include structural units represented by the following formulas (18) to (24). The structural unit represented by formula (12) may also be a structure in which the structural units represented by formulas (18) to (24) below are respectively repeated. The structural unit represented by formula (12) may be one of these alone or a combination of two or more different types.

[0066]

[0067]

[0068]

[0069]

[0070]

[0071]

[0072] More specifically, the structural unit represented by the formula (13) includes structural units represented by the following formulas (25) and (26). The structural unit represented by the formula (13) may also be a structure in which structural units represented by the following formulas (27) and (28) are respectively repeated. The structural unit represented by the formula (13) may be one of these alone or a combination of two or more different types.

[0073]

[0074] More specifically, examples of the structural unit represented by formula (14) include structural units represented by the following formulas (27) and (28). The structural unit represented by formula (14) may also be a structure in which the structural units represented by formula (27) and formula (28) are respectively repeated. The structural unit represented by formula (14) may be one of these alone or a combination of two or more different types.

[0075]

[0076] Preferred examples of the styrene copolymer (C) include polymers or copolymers obtained by polymerizing or copolymerizing one or more styrene monomers such as styrene, vinyltoluene, α-methylstyrene, isopropenyltoluene, divinylbenzene, and allylstyrene.

[0077] More specific examples of the styrene polymer (C) include styrene-butadiene block copolymers such as methylstyrene (ethylene / butylene) methylstyrene block copolymer, methylstyrene (ethylene-ethylene / propylene) methylstyrene block copolymer, styrene-isoprene block copolymer, styrene-isoprene-styrene block copolymer, styrene (ethylene / butylene) styrene block copolymer, styrene (ethylene-ethylene / propylene) styrene block copolymer, styrene-butadiene-styrene block copolymer, styrene-isobutylene-styrene block copolymer, styrene (butadiene / butylene) styrene block copolymer, and hydrogenated products of at least a portion of these.

[0078] As the styrene-based polymer (C), commercially available products may be used, such as Tuftec P1500, Tuftec H1041, and Tuftec H1517 manufactured by Asahi Kasei Corporation, and Asaprene T437 manufactured by Asahi Kasei Corporation.

[0079] As the styrene-based polymer (C), the above-exemplified styrene-based polymers may be used alone or in combination of two or more.

[0080] The styrene polymer (C) preferably has a weight-average molecular weight of 1,000 to 300,000, more preferably 10,000 to 200,000. If the molecular weight is too low, the glass transition temperature of the cured product of the resin composition tends to decrease, and the heat resistance tends to decrease. If the molecular weight is too high, the viscosity of the resin composition when made into a varnish or during heat molding tends to become too high. The weight-average molecular weight may be measured by a general molecular weight measurement method, and specific examples include values ​​measured using gel permeation chromatography (GPC).

[0081] (Inorganic Filler) The resin composition may contain an inorganic filler as needed, as long as the effects of the present invention are not impaired. Furthermore, it is preferable to contain the inorganic filler in order to improve the heat resistance of the cured product of the resin composition. The inorganic filler is not particularly limited as long as it can be used as an inorganic filler contained in the resin composition. Examples of the inorganic filler include metal oxide fillers such as silica filler, alumina filler, titanium oxide filler, magnesium oxide filler, and mica filler; metal hydroxide fillers such as magnesium hydroxide filler and aluminum hydroxide filler; talc filler, aluminum borate filler, barium sulfate filler, aluminum nitride filler, boron nitride filler, barium titanate filler, strontium titanate filler, calcium titanate filler, magnesium carbonate filler such as anhydrous magnesium carbonate filler, calcium carbonate filler, and molybdate fillers such as zinc molybdate filler, calcium molybdate filler, and magnesium molybdate filler. Among these, silica filler, metal hydroxide fillers such as magnesium hydroxide filler and aluminum hydroxide filler, aluminum oxide filler, boron nitride filler, strontium titanate filler, calcium titanate filler, and molybdate filler are preferred, and silica filler and zinc molybdate filler are more preferred.The silica filler is not particularly limited, and examples thereof include crushed silica, spherical silica, and silica particles, with spherical silica being preferred.Furthermore, the inorganic filler may be used alone or in combination of two or more.Furthermore, when the inorganic filler is used in combination of two or more, it is preferred to use a silica filler and a zinc molybdate filler in combination.

[0082] The inorganic filler may be a surface-treated or untreated inorganic filler. Examples of the surface treatment include treatment with a silane coupling agent.

[0083] The silane coupling agent is not particularly limited, and examples thereof include silane coupling agents having at least one functional group selected from the group consisting of vinyl group, styryl group, methacryloyl group, acryloyl group, phenylamino group, isocyanurate group, ureido group, mercapto group, isocyanate group, epoxy group, and acid anhydride group. That is, the silane coupling agent has at least one reactive functional group selected from vinyl group, styryl group, methacryloyl group, acryloyl group, phenylamino group, isocyanurate group, ureido group, mercapto group, isocyanate group, epoxy group, and acid anhydride group, and further includes compounds having a hydrolyzable group such as a methoxy group or an ethoxy group.

[0084] Examples of the silane coupling agent include those having a vinyl group, such as vinyltriethoxysilane and vinyltrimethoxysilane. Examples of the silane coupling agent include those having a styryl group, such as p-styryltrimethoxysilane and p-styryltriethoxysilane. Examples of the silane coupling agent include those having a methacryloyl group, such as 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, and 3-methacryloxypropylethyldiethoxysilane. Examples of the silane coupling agent include those having an acryloyl group, such as 3-acryloxypropyltrimethoxysilane and 3-acryloxypropyltriethoxysilane. Examples of the silane coupling agent include those having a phenylamino group, such as N-phenyl-3-aminopropyltrimethoxysilane and N-phenyl-3-aminopropyltriethoxysilane.

[0085] The average particle size of the inorganic filler is not particularly limited, and is preferably 0.05 to 10 μm, and more preferably 0.1 to 8 μm. Here, the average particle size refers to the volume average particle size. The volume average particle size can be measured, for example, by a laser diffraction method.

[0086] (Content) The content of the maleimide compound (A) is preferably 30 to 80 parts by mass, and more preferably 35 to 65 parts by mass, per 100 parts by mass of the total of the maleimide compound (A) and the benzoxazine compound (B). When the content of the maleimide compound (A) is within the above range, a resin composition that has a low thermal expansion coefficient and a cured product with high plating adhesion can be more suitably obtained. This is thought to be because when the content of the maleimide compound (A) is within the above range, the effects achieved by containing the maleimide compound (A) and the effects achieved by containing the benzoxazine compound (B) can each be fully exerted.

[0087] The content of the maleimide compound (A) is preferably 20 to 60 parts by mass, and more preferably 40 to 60 parts by mass, relative to 100 parts by mass in total of the maleimide compound (A), the benzoxazine compound (B), and the styrene-based polymer (C).

[0088] The content of the benzoxazine compound (B) is preferably 20 to 40 parts by mass, and more preferably 25 to 35 parts by mass, relative to 100 parts by mass in total of the maleimide compound (A), the benzoxazine compound (B), and the styrene-based polymer (C).

[0089] The content of the styrene-based polymer (C) is preferably 15 to 40 parts by mass, and more preferably 25 to 40 parts by mass, relative to 100 parts by mass in total of the maleimide compound (A), the benzoxazine compound (B), and the styrene-based polymer (C).

[0090] When the contents of the maleimide compound (A), the benzoxazine compound (B), and the styrene-based polymer (C) are each within the above ranges, a resin composition can be more suitably obtained that has a low thermal expansion coefficient and a cured product with high plating adhesion. This is thought to be because, when the contents of the maleimide compound (A), the benzoxazine compound (B), and the styrene-based polymer (C) are each within the above ranges, the effects achieved by containing the maleimide compound (A), the effects achieved by containing the benzoxazine compound (B), and the effects achieved by containing the styrene-based polymer (C) can all be fully exerted.

[0091] As described above, the resin composition may contain the inorganic filler. When the resin composition contains the inorganic filler, the content of the inorganic filler is preferably 50 to 250 parts by mass, and more preferably 100 to 200 parts by mass, relative to 100 parts by mass of the total of the maleimide compound (A), the benzoxazine compound (B), and the styrene-based polymer (C).

[0092] (Organic Component) The resin composition according to the present embodiment may contain, as necessary, an organic component other than the maleimide compound (A), the benzoxazine compound (B), and the styrene-based polymer (C), as long as the effects of the present invention are not impaired. Here, the organic component may react with or not react with at least one of the maleimide compound (A), the benzoxazine compound (B), and the styrene-based polymer (C). Examples of the organic component include a maleimide compound (D) different from the maleimide compound (A), a benzoxazine compound (E) different from the benzoxazine compound (B), an epoxy compound, a methacrylate compound, an acrylate compound, a vinyl compound, a cyanate ester compound, an active ester compound, and an allyl compound. That is, the resin composition further contains an organic component other than the maleimide compound (A), the benzoxazine compound (B), and the styrene-based polymer (C), and the organic component may contain at least one selected from the group consisting of a maleimide compound (D) different from the maleimide compound (A), a benzoxazine compound (E) different from the benzoxazine compound (B), an epoxy compound, a methacrylate compound, an acrylate compound, a vinyl compound, a cyanate ester compound, an active ester compound, and an allyl compound.

[0093] The maleimide compound (D) is a maleimide compound that has a maleimide group in the molecule but does not have the indane structure represented by formula (1) in the molecule. Examples of the maleimide compound (D) include maleimide compounds that have one or more maleimide groups in the molecule and modified maleimide compounds. The maleimide compound (D) is not particularly limited as long as it is a maleimide compound that has one or more maleimide groups in the molecule but does not have the indane structure represented by formula (1) in the molecule. Examples of the maleimide compound (D) include phenylmaleimide compounds such as 4,4'-diphenylmethane bismaleimide, phenylmethane maleimide, m-phenylene bismaleimide, bisphenol A diphenyl ether bismaleimide, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, and biphenylaralkyl polymaleimide compounds, as well as N-alkyl bismaleimide compounds having an aliphatic skeleton. Examples of the modified maleimide compound include modified maleimide compounds in which a portion of the molecule is modified with an amine compound, and modified maleimide compounds in which a portion of the molecule is modified with a silicone compound. As the maleimide compound (D), commercially available products may be used. For example, the solid content of MIR-3000-70MT and the solid content of MIR-5000-60T manufactured by Nippon Kayaku Co., Ltd., BMI-2300, BMI-4000, and BMI-5100 manufactured by Daiwa Chemical Industry Co., Ltd., and BMI-689, BMI-1500, BMI-3000J, and BMI-5000 manufactured by Designer Molecules Inc. may be used.

[0094] The benzoxazine compound (E) is a benzoxazine compound other than the benzoxazine compound (B) [such as the benzoxazine compound (B1) (such as the benzoxazine compound (B4)), the benzoxazine compound (B2), and the benzoxazine compound (B3)]. The benzoxazine compound (E) is not particularly limited as long as it is a benzoxazine compound having a benzoxazine group in the molecule and is a benzoxazine compound other than the benzoxazine compound (B). Examples of the benzoxazine compound (E) include a benzoxazine compound having a phenolphthalein structure in the molecule (phenolphthalein-type benzoxazine compound), a bisphenol F-type benzoxazine compound, and a diaminodiphenylmethane (DDM)-type benzoxazine compound. More specific examples of the other benzoxazine compounds include 3,3'-(methylene-1,4-diphenylene)bis(3,4-dihydro-2H-1,3-benzoxazine) (P-d type benzoxazine compound), 2,2-bis(3,4-dihydro-2H-3-phenyl-1,3-benzoxazine)methane (F-a type benzoxazine compound), and oxydianiline (ODA) type benzoxazine.

[0095] The epoxy compound is a compound having an epoxy group in the molecule, and specific examples thereof include bisphenol-type epoxy compounds such as bisphenol A-type epoxy compounds, phenol novolac-type epoxy compounds, cresol novolac-type epoxy compounds, dicyclopentadiene-type epoxy compounds, bisphenol A novolac-type epoxy compounds, biphenyl aralkyl-type epoxy compounds, and naphthalene ring-containing epoxy compounds. The epoxy compound also includes epoxy resins, which are polymers of the above-mentioned epoxy compounds.

[0096] The methacrylate compound is a compound having a methacryloyl group in the molecule, and examples thereof include monofunctional methacrylate compounds having one methacryloyl group in the molecule and polyfunctional methacrylate compounds having two or more methacryloyl groups in the molecule. Examples of the monofunctional methacrylate compound include methyl methacrylate, ethyl methacrylate, propyl methacrylate, and butyl methacrylate. Examples of the polyfunctional methacrylate compound include dimethacrylate compounds such as tricyclodecane dimethanol dimethacrylate (DCP).

[0097] The acrylate compound is a compound having an acryloyl group in the molecule, and examples thereof include monofunctional acrylate compounds having one acryloyl group in the molecule and polyfunctional acrylate compounds having two or more acryloyl groups in the molecule. Examples of the monofunctional acrylate compound include methyl acrylate, ethyl acrylate, propyl acrylate, and butyl acrylate. Examples of the polyfunctional acrylate compound include diacrylate compounds such as tricyclodecane dimethanol diacrylate.

[0098] The vinyl compound is a compound having a vinyl group in its molecule, and examples thereof include monofunctional vinyl compounds (monovinyl compounds) having one vinyl group in their molecule, and polyfunctional vinyl compounds having two or more vinyl groups in their molecule. Examples of the polyfunctional vinyl compound include divinylbenzene, curable polybutadiene having a carbon-carbon unsaturated double bond in its molecule, butadiene-styrene copolymers other than the styrene-based polymers, polyphenylene ether compounds having vinylbenzyl groups (ethenylbenzyl groups) at their terminals, and modified polyphenylene ethers in which the terminal hydroxyl groups of polyphenylene ethers have been modified with methacrylic groups. Furthermore, examples of butadiene-styrene copolymers other than the styrene-based polymers include curable butadiene-styrene copolymers having a carbon-carbon unsaturated double bond in their molecule that is liquid at 25°C, curable butadiene-styrene random copolymers having a carbon-carbon unsaturated double bond in their molecule, and curable butadiene-styrene random copolymers having a carbon-carbon unsaturated double bond in their molecule that is liquid at 25°C.

[0099] The cyanate ester compound is a compound having a cyanate group in the molecule, and examples thereof include 2,2-bis(4-cyanatephenyl)propane, bis(3,5-dimethyl-4-cyanatephenyl)methane, and 2,2-bis(4-cyanatephenyl)ethane.

[0100] The active ester compound is a compound having an ester group with high reactivity in the molecule, and examples thereof include benzenecarboxylic acid active ester, benzenedicarboxylic acid active ester, benzenetricarboxylic acid active ester, benzenetetracarboxylic acid active ester, naphthalenecarboxylic acid active ester, naphthalenedicarboxylic acid active ester, naphthalenetricarboxylic acid active ester, naphthalenetetracarboxylic acid active ester, fluorenecarboxylic acid active ester, fluorenedicarboxylic acid active ester, fluorenetricarboxylic acid active ester, and fluorenetetracarboxylic acid active ester.

[0101] The allyl compound is a compound having an allyl group in the molecule, and examples thereof include triallyl isocyanurate compounds such as triallyl isocyanurate (TAIC), diallyl bisphenol compounds, allyl epoxy compounds, and diallyl phthalate (DAP).

[0102] The organic component may be used alone or in combination of two or more kinds.

[0103] The weight-average molecular weight of the organic component is not particularly limited, but is preferably 100 to 5000, more preferably 100 to 4000, and even more preferably 100 to 3000. If the weight-average molecular weight of the organic component is too low, the organic component may be more likely to volatilize from the resin composition's blended components. Furthermore, if the weight-average molecular weight of the organic component is too high, the viscosity of the resin composition varnish or the melt viscosity during heat molding may become too high, potentially resulting in poor appearance and moldability when B-staged. Therefore, when the weight-average molecular weight of the organic component is within this range, a resin composition with excellent heat resistance and moldability of the cured product can be obtained. This is thought to be because the resin composition can be cured appropriately. The weight-average molecular weight may be measured using a common molecular weight measurement method, specifically, a value measured using gel permeation chromatography (GPC), etc.

[0104] The organic component has an average number of functional groups per molecule that contribute to the reaction during curing of the resin composition (number of functional groups), which varies depending on the weight-average molecular weight of the organic component, but is preferably 1 to 20, and more preferably 2 to 18. If the number of functional groups is too small, it tends to be difficult to obtain sufficient heat resistance of the cured product. On the other hand, if the number of functional groups is too large, the reactivity becomes too high, which may cause problems such as reduced shelf life and reduced fluidity of the resin composition.

[0105] (Other Components) The resin composition may contain components (other components) other than the maleimide compound (A) and the benzoxazine compound (B), as long as the effects of the present invention are not impaired. As described above, the resin composition may contain the styrene-based polymer (C), the inorganic filler, and the organic component as the other components. Examples of the other components include, in addition to the styrene-based polymer (C), the inorganic filler, and the organic component, additives such as flame retardants, reaction initiators, curing accelerators, catalysts, polymerization retarders, polymerization inhibitors, dispersants, leveling agents, coupling agents, defoamers, antioxidants, heat stabilizers, antistatic agents, UV absorbers, dyes, pigments, and lubricants.

[0106] As described above, the resin composition according to this embodiment may contain a flame retardant. By including a flame retardant, the flame retardancy of the cured resin composition can be improved. The flame retardant is not particularly limited. Specifically, in fields where halogen-based flame retardants such as bromine-based flame retardants are used, for example, ethylene dipentabromobenzene, ethylene bistetrabromoimide, decabromodiphenyl oxide, tetradecabromodiphenoxybenzene, and bromostyrene-based compounds that react with the polymerizable compounds, which have melting points of 300°C or higher, are preferred. It is believed that the use of a halogen-based flame retardant can suppress halogen elimination at high temperatures and thus suppress a decrease in heat resistance. Furthermore, in fields where halogen-free materials are required, phosphorus-containing flame retardants (phosphorus-based flame retardants) are sometimes used. The phosphorus-based flame retardant is not particularly limited, but examples thereof include phosphate ester-based flame retardants, phosphazene-based flame retardants, bisdiphenylphosphine oxide-based flame retardants, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO)-based flame retardants, and phosphinate-based flame retardants. Specific examples of phosphate ester-based flame retardants include condensed phosphate esters of dixylenyl phosphate. Specific examples of phosphazene-based flame retardants include phenoxyphosphazene. Specific examples of bisdiphenylphosphine oxide-based flame retardants include xylylenebisdiphenylphosphine oxide. Specific examples of DOPO-based flame retardants include hydrocarbons having two DOPO groups in the molecule (DOPO derivative compounds). Specific examples of phosphinate-based flame retardants include metal phosphinates of aluminum dialkylphosphinates. As the flame retardant, each of the exemplified flame retardants may be used alone or in combination of two or more kinds.

[0107] As described above, the resin composition according to this embodiment may contain a reaction initiator. The reaction initiator is not particularly limited as long as it can accelerate the curing reaction of the resin composition, and examples thereof include peroxides and organic azo compounds. Examples of peroxides include α,α'-di(t-butylperoxy)diisopropylbenzene (PBP), 2,5-dimethyl-2,5-di(t-butylperoxy)-3-hexyne, and benzoyl peroxide. Examples of organic azo compounds include azobisisobutyronitrile. If necessary, a metal carboxylate or the like can be used in combination. This further accelerates the curing reaction. Among these, α,α'-di(t-butylperoxy)diisopropylbenzene is preferred. Because α,α'-di(t-butylperoxy)diisopropylbenzene has a relatively high reaction initiation temperature, it can suppress acceleration of the curing reaction when curing is not required, such as during prepreg drying, thereby suppressing deterioration in the shelf life of the resin composition. Furthermore, since α,α'-di(t-butylperoxy)diisopropylbenzene has low volatility, it does not volatilize during drying or storage of the prepreg, and has good stability. The reaction initiators may be used alone or in combination of two or more.

[0108] As described above, the resin composition according to this embodiment may contain a curing accelerator. The curing accelerator is not particularly limited as long as it can accelerate the curing reaction of the resin composition. Specific examples of the curing accelerator include imidazoles and their derivatives, organophosphorus compounds, amines such as secondary amines and tertiary amines, quaternary ammonium salts, organoboron compounds, and metal soaps. Examples of the imidazoles include 2-ethyl-4-methylimidazole (2E4MZ), 2-methylimidazole, 2-phenyl-4-methylimidazole, 2-phenylimidazole, and 1-benzyl-2-methylimidazole. Examples of the organophosphorus compounds include triphenylphosphine, diphenylphosphine, phenylphosphine, tributylphosphine, and trimethylphosphine. Examples of the amines include dimethylbenzylamine, triethylenediamine, triethanolamine, and 1,8-diaza-bicyclo(5,4,0)undecene-7 (DBU). Examples of the quaternary ammonium salts include tetrabutylammonium bromide. Examples of the organoboron compounds include tetraphenylboron salts such as 2-ethyl-4-methylimidazole tetraphenylborate, and tetra-substituted phosphonium tetra-substituted borates such as tetraphenylphosphonium ethyltriphenylborate. The metal soap refers to a fatty acid metal salt, and may be either a linear fatty acid metal salt or a cyclic fatty acid metal salt. Specific examples of the metal soap include linear fatty acid metal salts and cyclic fatty acid metal salts having 6 to 10 carbon atoms. More specifically, examples of the curing accelerator include aliphatic metal salts composed of linear fatty acids such as stearic acid, lauric acid, ricinoleic acid, and octylic acid, or cyclic fatty acids such as naphthenic acid, and metals such as lithium, magnesium, calcium, barium, copper, and zinc. For example, zinc octylate is included. The curing accelerators may be used alone or in combination of two or more.

[0109] As described above, the resin composition according to this embodiment may contain a silane coupling agent. The silane coupling agent may be contained in the resin composition, or may be contained as a silane coupling agent that has been surface-treated in advance on an inorganic filler contained in the resin composition. Among these, the silane coupling agent is preferably contained as a silane coupling agent that has been surface-treated in advance on an inorganic filler, and it is more preferable to contain the silane coupling agent in advance on an inorganic filler in this way, and further to contain the silane coupling agent in the resin composition. In addition, in the case of a prepreg, the prepreg may contain the silane coupling agent that has been surface-treated in advance on a fibrous substrate. Examples of the silane coupling agent include the same silane coupling agents as those used when surface-treating the inorganic filler described above.

[0110] The resin composition according to this embodiment is a resin composition that can yield a cured product with a low thermal expansion coefficient and high plating adhesion. Furthermore, in order to suppress losses due to increased resistance associated with miniaturization of wiring, the insulating layer provided on the wiring board is also required to have lower dielectric properties such as dielectric loss tangent. The resin composition is a resin composition that can yield a cured product with a low thermal expansion coefficient, high plating adhesion, and also a low dielectric loss tangent.

[0111] Wiring boards used in various electronic devices are also required to be resistant to changes in the external environment, etc. For example, to enable the wiring board to be used even in relatively high-temperature environments, the substrate material for constituting the insulating layer of the wiring board is required to produce a cured product with excellent heat resistance, such as a high glass transition temperature. It is also required that the insulating layer provided on the wiring board does not deform even in relatively high-temperature environments. Since a high glass transition temperature of the insulating layer suppresses this deformation, the substrate material for constituting the insulating layer of the wiring board is required to have a high glass transition temperature. The resin composition according to this embodiment is a resin composition that not only has a low thermal expansion coefficient and high plating adhesion, but also produces a cured product with a high glass transition temperature.

[0112] Electronic devices, particularly small portable devices such as mobile communication terminals and laptops, are rapidly becoming more diverse, more powerful, thinner, and smaller. Accordingly, the wiring boards used in these products are also required to have finer conductor wiring, more multilayered conductor wiring layers, thinner wiring, and improved mechanical properties. Therefore, even if the wiring provided on the wiring board is finer, it is also required that the wiring does not peel off from the insulating layer. To meet this requirement, the wiring board is required to have high adhesion between the wiring and the insulating layer. Therefore, metal-clad laminates are required to have high adhesion between the metal foil and the insulating layer, and substrate materials for forming the insulating layer of wiring boards are required to produce cured products that have excellent adhesion to the metal foil. Furthermore, as mentioned above, wiring boards are required to be multilayered, and when the insulating layer is thus constructed in multiple layers, high interlayer adhesion is also required to prevent interlayer delamination. Therefore, substrate materials for forming the insulating layer of wiring boards are required to produce cured products that have excellent adhesion between adjacent cured products, i.e., excellent interlayer adhesion. The resin composition according to this embodiment is a resin composition that not only has a low thermal expansion coefficient and high plating adhesion, but also gives a cured product that is excellent in adhesion to metal foil and interlayer adhesion.

[0113] As described above, the insulating layer of a wiring board used in various electronic devices is required to be able to appropriately perform electroless plating and electrolytic plating after removing smears (residues) generated by drilling using a drill, laser, or the like. Specifically, the insulating layer of a wiring board is required to have excellent desmear properties (for example, to be able to appropriately remove smears using permanganic acid or the like while suppressing damage to the insulating layer of the wiring board). For this reason, a substrate material for forming the insulating layer of a wiring board is required to provide a cured product with excellent desmear properties. The resin composition according to this embodiment is a resin composition that not only has a low thermal expansion coefficient and high plating adhesion, but also provides a cured product with excellent desmear properties.

[0114] The resin composition according to this embodiment is a resin composition that can give a cured product that has a low thermal expansion coefficient and excellent plating adhesion. Furthermore, the resin composition according to this embodiment is a resin composition that can give a cured product that not only has a low thermal expansion coefficient and excellent plating adhesion, but also has a low dielectric tangent, a high glass transition temperature, and excellent adhesion to metal foil, interlayer adhesion, and desmear properties.

[0115] (Uses) The resin composition is used to produce a prepreg, as described below, and to form a resin layer provided in a resin-coated metal foil or a resin-coated film, and an insulating layer provided in a metal-clad laminate or a wiring board.

[0116] (Production Method) The method for producing the resin composition is not particularly limited, and examples thereof include a method of mixing the maleimide compound (A), the benzoxazine compound (B), the styrene-based polymer (C), and, if necessary, components other than the maleimide compound (A), the benzoxazine compound (B), and the styrene-based polymer (C) so as to achieve a predetermined content. In addition, in the case of obtaining a varnish-like composition containing an organic solvent, the method described below can be used.

[0117] [Prepreg, metal-clad laminate, wiring board, resin-coated metal foil, and resin-coated film] By using the resin composition according to this embodiment, a prepreg, a metal-clad laminate, a wiring board, a resin-coated metal foil, and a resin-coated film can be obtained as follows.

[0118] (Prepreg) FIG. 1 is a schematic cross-sectional view showing an example of a prepreg 1 according to an embodiment of the present invention.

[0119] 1, the prepreg 1 according to this embodiment comprises the resin composition or a semi-cured product of the resin composition 2, and a fibrous base material 3. This prepreg 1 comprises the resin composition or a semi-cured product of the resin composition 2, and the fibrous base material 3 present in the resin composition or the semi-cured product of the resin composition 2.

[0120] In this embodiment, the semi-cured product refers to a resin composition that has been partially cured to the extent that it can be further cured. That is, the semi-cured product refers to a resin composition that has been semi-cured (B-staged). For example, when a resin composition is heated, the viscosity initially gradually decreases, and then curing begins, and the viscosity gradually increases. In such a case, the semi-cured state may refer to a state between when the viscosity starts to increase and when the composition is completely cured.

[0121] The prepreg obtained using the resin composition according to this embodiment may comprise a semi-cured product of the resin composition as described above, or may comprise the uncured resin composition itself. That is, it may be a prepreg comprising a semi-cured product of the resin composition (the resin composition in B stage) and a fibrous base material, or a prepreg comprising the resin composition before curing (the resin composition in A stage) and a fibrous base material. Furthermore, the resin composition or the semi-cured product of the resin composition may be the resin composition that has been dried or heat-dried.

[0122] When producing the prepreg, the resin composition 2 is often prepared in a varnish form and used to impregnate the fibrous base material 3, which is a base material for forming the prepreg. That is, the resin composition 2 is usually often a resin varnish prepared in a varnish form. Such a varnish-like resin composition (resin varnish) is prepared, for example, as follows.

[0123] First, each component that is soluble in an organic solvent is added to the organic solvent and dissolved therein. Heating may be performed as necessary. Subsequently, components that are insoluble in the organic solvent are added as needed, and the mixture is dispersed using a ball mill, bead mill, planetary mixer, roll mill, or the like until a predetermined dispersion state is achieved, thereby preparing a varnish-like resin composition. The organic solvent used here is not particularly limited as long as it dissolves the maleimide compound (A), the benzoxazine compound (B), the styrene-based polymer (C), and the like and does not inhibit the curing reaction. Specific examples include toluene and methyl ethyl ketone (MEK).

[0124] Specific examples of the fibrous substrate include glass cloth, aramid cloth, polyester cloth, glass nonwoven fabric, aramid nonwoven fabric, polyester nonwoven fabric, pulp paper, and linter paper. Glass cloth can be used to obtain a laminate with excellent mechanical strength, and flattened glass cloth is particularly preferred. A specific example of the flattening process is a method in which glass cloth is continuously pressed with a press roll at an appropriate pressure to compress the yarns flat. The thickness of commonly used fibrous substrates is, for example, 0.01 mm or more and 0.3 mm or less. The glass fibers constituting the glass cloth are not particularly limited, and examples include Q glass, NE glass, E glass, S glass, T glass, L glass, and L2 glass. The surface of the fibrous substrate may be treated with a silane coupling agent. The silane coupling agent is not particularly limited, but examples thereof include silane coupling agents having at least one group selected from the group consisting of a vinyl group, an acryloyl group, a methacryloyl group, a styryl group, an amino group, and an epoxy group in the molecule.

[0125] The method for producing the prepreg is not particularly limited as long as it can produce the prepreg. Specifically, when producing the prepreg, the resin composition according to the present embodiment is often prepared in the form of a varnish, as described above, and used as a resin varnish.

[0126] Specific examples of methods for producing the prepreg 1 include a method in which the resin composition 2, for example, a resin composition 2 prepared in a varnish form, is impregnated into a fibrous substrate 3, followed by drying. The resin composition 2 is impregnated into the fibrous substrate 3 by immersion, coating, or the like. Impregnation can be repeated multiple times as necessary. In this case, by repeating the impregnation using multiple resin compositions with different compositions and concentrations, it is also possible to adjust the final composition and impregnation amount to the desired one.

[0127] The fibrous substrate 3 impregnated with the resin composition (resin varnish) 2 is heated under desired conditions, for example, at 40°C to 180°C for 1 minute to 10 minutes. This heating process results in a prepreg 1 in an uncured (A-stage) or semi-cured (B-stage) state. The heating process also volatilizes the organic solvent from the resin varnish, reducing or eliminating the organic solvent.

[0128] (Metal-clad laminate) FIG. 2 is a schematic cross-sectional view showing an example of a metal-clad laminate 11 according to an embodiment of the present invention.

[0129] As shown in FIG. 2 , the metal-clad laminate 11 according to this embodiment includes an insulating layer 12 containing a cured product of the resin composition and a metal foil 13 disposed on the insulating layer 12. Examples of the metal-clad laminate 11 include a metal-clad laminate composed of an insulating layer 12 containing a cured product of the prepreg 1 shown in FIG. 1 and a metal foil 13 laminated together with the insulating layer 12. The insulating layer 12 may be composed of a cured product of the resin composition or a cured product of the prepreg. The thickness of the metal foil 13 varies depending on the performance required of the final wiring board and is not particularly limited. The thickness of the metal foil 13 can be appropriately set depending on the desired purpose, and is preferably, for example, 0.2 to 70 μm. Examples of the metal foil 13 include copper foil and aluminum foil. When the metal foil is thin, it may be a carrier-attached copper foil equipped with a release layer and a carrier to improve handling.

[0130] The method for producing the metal-clad laminate 11 is not particularly limited as long as it can produce the metal-clad laminate 11. Specifically, a method for producing the metal-clad laminate 11 using the prepreg 1 can be used. Examples of such a method include stacking one or more prepregs 1, placing a metal foil 13 such as copper foil on both sides or one side of the prepreg 1, and then heat-pressing and molding the metal foil 13 and the prepreg 1 to form an integrated laminate. That is, the metal-clad laminate 11 can be obtained by laminating the metal foil 13 on the prepreg 1 and then heat-pressing and molding the laminate. The heat-pressing conditions can be appropriately set depending on the thickness of the metal-clad laminate 11, the type of resin composition contained in the prepreg 1, and other factors. For example, the temperature can be 170 to 230°C, the pressure can be 0.5 to 5 MPa, and the time can be 60 to 150 minutes. The metal-clad laminate can also be produced without using a prepreg. For example, a method may be used in which a varnish-like resin composition is applied onto a metal foil to form a layer containing the resin composition on the metal foil, and then the layer is heated and pressed.

[0131] (Wiring Board) FIG. 3 is a schematic cross-sectional view showing an example of a wiring board 21 according to an embodiment of the present invention.

[0132] As shown in Fig. 3, wiring board 21 according to this embodiment has insulating layer 12 containing a cured product of the resin composition, and wiring 14 provided on insulating layer 12. Examples of wiring board 21 include a wiring board configured from insulating layer 12 used by curing prepreg 1 shown in Fig. 1, and wiring 14 laminated together with insulating layer 12 and formed by partially removing metal foil 13. Furthermore, insulating layer 12 may be made of a cured product of the resin composition, or may be made of a cured product of the prepreg.

[0133] The method for manufacturing the wiring board 21 is not particularly limited as long as the wiring board 21 can be manufactured. Specific examples include a method of manufacturing the wiring board 21 using the prepreg 1. Examples of this method include a method of manufacturing the wiring board 21 in which wiring is provided as a circuit on the surface of the insulating layer 12 by etching the metal foil 13 on the surface of the metal-clad laminate 11 manufactured as described above. That is, the wiring board 21 is obtained by forming a circuit by partially removing the metal foil 13 on the surface of the metal-clad laminate 11. In addition to the above methods, examples of the method for forming a circuit include circuit formation by a semi-additive process (SAP) or a modified semi-additive process (MSAP).

[0134] (Resin-Coated Metal Foil) FIG. 4 is a schematic cross-sectional view showing an example of a resin-coated metal foil 31 according to this embodiment.

[0135] As shown in Fig. 4, the resin-coated metal foil 31 according to this embodiment comprises a resin layer 32 containing the resin composition or a semi-cured product of the resin composition, and a metal foil 13. The resin-coated metal foil 31 has the metal foil 13 on the surface of the resin layer 32. That is, the resin-coated metal foil 31 comprises the resin layer 32 and the metal foil 13 laminated together with the resin layer 32. The resin-coated metal foil 31 may also comprise another layer between the resin layer 32 and the metal foil 13.

[0136] The resin layer 32 may contain a semi-cured product of the resin composition as described above, or may contain the uncured resin composition. That is, the resin-coated metal foil 31 may comprise a resin layer containing a semi-cured product of the resin composition (the resin composition in B-stage) and a metal foil, or a resin layer containing the resin composition before curing (the resin composition in A-stage) and a metal foil. The resin layer may contain the resin composition or a semi-cured product of the resin composition, and may or may not contain a fibrous substrate. The resin composition or the semi-cured product of the resin composition may be the resin composition that has been dried or heat-dried. The fibrous substrate may be the same as the fibrous substrate of a prepreg.

[0137] The metal foil may be any metal foil used in a metal-clad laminate or a resin-coated metal foil, and examples of the metal foil include copper foil and aluminum foil.

[0138] The resin-coated metal foil 31 may be provided with a cover film or the like as necessary. By providing a cover film, it is possible to prevent the inclusion of foreign matter, etc. The cover film is not particularly limited, but examples thereof include polyolefin films, polyester films, polymethylpentene films, and films formed by providing these films with a release agent layer.

[0139] The method for producing the resin-coated metal foil 31 is not particularly limited as long as the resin-coated metal foil 31 can be produced. Examples of the method for producing the resin-coated metal foil 31 include a method of applying the varnish-like resin composition (resin varnish) to the metal foil 13 and heating the applied resin composition. The varnish-like resin composition is applied to the metal foil 13 using, for example, a bar coater. The applied resin composition is heated, for example, at 40°C or higher and 180°C or lower for 0.1 minutes or longer and 10 minutes or shorter. The heated resin composition is formed on the metal foil 13 as an uncured resin layer 32. The heating volatilizes the organic solvent from the resin varnish, thereby reducing or removing the organic solvent.

[0140] (Resin-Coated Film) FIG. 5 is a schematic cross-sectional view showing an example of a resin-coated film 41 according to this embodiment.

[0141] 5 , the resin-coated film 41 according to this embodiment includes a resin layer 42 containing the resin composition or a semi-cured product of the resin composition, and a support film 43. The resin-coated film 41 includes the resin layer 42 and the support film 43 laminated together with the resin layer 42. The resin-coated film 41 may also include another layer between the resin layer 42 and the support film 43.

[0142] The resin layer 42 may contain a semi-cured product of the resin composition as described above, or may contain the uncured resin composition. That is, the resin-coated film 41 may comprise a resin layer containing a semi-cured product of the resin composition (the resin composition in B-stage) and a support film, or a resin-coated film comprising a resin layer containing the resin composition before curing (the resin composition in A-stage) and a support film. The resin layer may contain the resin composition or a semi-cured product of the resin composition, and may or may not contain a fibrous substrate. The resin composition or the semi-cured product of the resin composition may be obtained by drying or heat-drying the resin composition. The fibrous substrate may be the same as the fibrous substrate of a prepreg.

[0143] Any support film used for a resin-coated film can be used without limitation as the support film 43. Examples of the support film include electrically insulating films such as polyester film, polyethylene terephthalate (PET) film, polyimide film, polyparabanic acid film, polyether ether ketone film, polyphenylene sulfide film, polyamide film, polycarbonate film, and polyarylate film.

[0144] The resin-coated film 41 may be provided with a cover film or the like as necessary. By providing a cover film, it is possible to prevent the inclusion of foreign matter, etc. The cover film is not particularly limited, but examples thereof include a polyolefin film, a polyester film, and a polymethylpentene film.

[0145] The support film and the cover film may be subjected to surface treatment such as matte treatment, corona treatment, release treatment, and roughening treatment, if necessary.

[0146] The method for producing the resin-coated film 41 is not particularly limited as long as it can produce the resin-coated film 41. Examples of methods for producing the resin-coated film 41 include a method in which the varnish-like resin composition (resin varnish) is applied to a support film 43 and heated. The varnish-like resin composition is applied to the support film 43 using, for example, a bar coater. The applied resin composition is heated, for example, at 40°C or higher and 180°C or lower for 0.1 minutes or longer and 10 minutes or shorter. The heated resin composition is formed on the support film 43 as an uncured resin layer 42. The heating volatilizes the organic solvent from the resin varnish, thereby reducing or removing the organic solvent.

[0147] When cured, the resin composition according to this embodiment forms a cured product with a low thermal expansion coefficient and high plating adhesion. Therefore, when cured, the prepreg forms a cured product with a low thermal expansion coefficient and high plating adhesion. The resin-coated metal foil and the resin-coated film are, respectively, resin-coated metal foil and resin-coated film, each having a resin layer that becomes an insulating layer containing the cured product when cured. The metal-clad laminate and the wiring board are, respectively, metal-clad laminate and wiring board, each having an insulating layer containing the cured product. The prepreg, the resin-coated film, the resin-coated metal foil, and the metal-clad laminate can be suitably used to manufacture the wiring board, for example, and can also be used to manufacture a multilayer wiring board. For example, a multilayer wiring board can be manufactured by laminating the resin-coated film on a wiring board and then peeling off the support film, or by laminating the resin-coated film on a wiring board after peeling off the support film. The resin-coated metal foil can be, for example, laminated on a wiring board, to manufacture a multilayer wiring board. In this way, by using the resin-coated film and the resin-coated metal foil, etc., it is possible to manufacture a multi-layer wiring board having an insulating layer containing the cured product.

[0148] As described above, this specification discloses various aspects of the technology, the main technologies of which are summarized below.

[0149] A resin composition according to a first aspect of the present invention is a resin composition containing a maleimide compound (A) having an indane structure represented by the following formula (1) in the molecule, a benzoxazine compound (B) having an allyl group in the molecule, and a styrene-based polymer (C) that is solid at 25°C:

[0150] In formula (1), each Rb independently represents an alkyl group having 1 to 10 carbon atoms, an alkyloxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a nitro group, a hydroxyl group, or a mercapto group; and r represents an integer of 0 to 3.

[0151] A resin composition according to a second aspect of the present invention is the resin composition according to the first aspect, wherein the maleimide compound (A) comprises a maleimide compound (A1) represented by the following formula (2):

[0152] In formula (2), each Ra independently represents an alkyl group having 1 to 10 carbon atoms, an alkyloxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a nitro group, a hydroxyl group, or a mercapto group; each Rb independently represents an alkyl group having 1 to 10 carbon atoms, an alkyloxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a nitro group, a hydroxyl group, or a mercapto group; q represents 0 to 4; r represents 0 to 3; and n represents 0.95 to 10.

[0153] A resin composition according to a third aspect of the present invention is the resin composition according to the first or second aspect of the present invention, wherein the benzoxazine compound (B) comprises at least one compound selected from the group consisting of a benzoxazine compound (B1) having a benzoxazine group represented by the following formula (3) in the molecule, a benzoxazine compound (B2) having a benzoxazine group represented by the following formula (4) in the molecule, and a benzoxazine compound (B3) having a benzoxazine group represented by the following formula (3) and a benzoxazine group represented by the following formula (4) in the molecule:

[0154] In formula (3), R 1 represents an allyl group, and p represents 1 to 4.

[0155] In formula (4), R 2 represents an allyl group.

[0156] A resin composition according to a fourth aspect of the present invention is the resin composition according to the third aspect of the present invention, wherein the benzoxazine compound (B1) comprises a benzoxazine compound (B4) represented by the following formula (5):

[0157] In formula (5), R 3 and R 4 represents an allyl group; X represents an ether bond or an alkylene group; q and r each independently represent 1 to 4.

[0158] A resin composition according to a fifth aspect of the present invention is the resin composition according to any one of the first to fourth aspects of the present invention, wherein the styrene polymer (C) comprises at least one selected from the group consisting of methylstyrene (ethylene / butylene) methylstyrene block copolymer, methylstyrene (ethylene-ethylene / propylene) methylstyrene block copolymer, styrene isoprene block copolymer, styrene isoprene styrene block copolymer, styrene (ethylene / butylene) styrene block copolymer, styrene (ethylene-ethylene / propylene) styrene block copolymer, styrene butadiene block copolymer, styrene isobutylene styrene block copolymer, styrene (butadiene / butylene) styrene block copolymer, and hydrogenated products of at least a portion thereof.

[0159] A resin composition according to a sixth aspect of the present invention is the resin composition according to any one of the first to fourth aspects of the present invention, wherein the styrene-based polymer (C) is at least partially hydrogenated.

[0160] A resin composition according to a seventh aspect of the present invention is the resin composition according to any one of the first to sixth aspects of the present invention, further comprising an organic component other than the maleimide compound (A), the benzoxazine compound (B), and the styrene-based polymer (C), wherein the organic component comprises at least one selected from the group consisting of a maleimide compound (D) different from the maleimide compound (A), a benzoxazine compound (E) different from the benzoxazine compound (B), an epoxy compound, a methacrylate compound, an acrylate compound, a vinyl compound, a cyanate ester compound, an active ester compound, and an allyl compound.

[0161] A resin composition according to an eighth aspect of the present invention is the resin composition according to any one of the first to seventh aspects of the present invention, wherein the content of the maleimide compound (A) is 30 to 80 parts by mass per 100 parts by mass of the total of the maleimide compound (A) and the benzoxazine compound (B).

[0162] A resin composition according to a ninth aspect of the present invention is the resin composition according to any one of the first to eighth aspects of the present invention, wherein the content of the maleimide compound (A) is 20 to 60 parts by mass per 100 parts by mass of the total of the maleimide compound (A), the benzoxazine compound (B), and the styrene-based polymer (C).

[0163] A resin composition according to a tenth aspect of the present invention is the resin composition according to any one of the first to ninth aspects of the present invention, wherein the content of the styrene-based polymer (C) is 15 to 40 parts by mass per 100 parts by mass of the total of the maleimide compound (A), the benzoxazine compound (B), and the styrene-based polymer (C).

[0164] A resin composition according to an eleventh aspect of the present invention is the resin composition according to any one of the first to tenth aspects of the present invention, further comprising an inorganic filler.

[0165] A resin composition according to a twelfth aspect of the present invention is the resin composition according to the eleventh aspect of the present invention, wherein the content of the inorganic filler is 50 to 250 parts by mass per 100 parts by mass of the total of the maleimide compound (A), the benzoxazine compound (B), and the styrene-based polymer (C).

[0166] A prepreg according to a thirteenth aspect of the present invention is a prepreg comprising the resin composition according to any one of the first to twelfth aspects of the present invention or a semi-cured product of the resin composition, and a fibrous base material.

[0167] The resin-coated film according to the fourteenth aspect of the present invention is a resin-coated film comprising a resin layer containing the resin composition according to any one of the first to twelfth aspects of the present invention or a semi-cured product of the resin composition, and a support film.

[0168] A resin-coated metal foil according to a fifteenth aspect of the present invention is a resin-coated metal foil comprising a resin layer containing the resin composition according to any one of the first to twelfth aspects of the present invention or a semi-cured product of the resin composition, and a metal foil.

[0169] A metal-clad laminate according to a sixteenth aspect of the present invention is a metal-clad laminate comprising an insulating layer containing a cured product of the resin composition according to any one of the first to twelfth aspects of the present invention, and a metal foil.

[0170] A metal-clad laminate according to a seventeenth aspect of the present invention is a metal-clad laminate comprising an insulating layer containing a cured product of the prepreg according to the thirteenth aspect of the present invention and a metal foil.

[0171] A wiring board according to an eighteenth aspect of the present invention is a wiring board comprising an insulating layer containing a cured product of the resin composition according to any one of the first to twelfth aspects of the present invention, and wiring.

[0172] A wiring board according to a nineteenth aspect of the present invention is a wiring board comprising an insulating layer containing a cured product of the prepreg according to the thirteenth aspect of the present invention and wiring.

[0173] According to the present invention, there is provided a resin composition that can give a cured product having a low thermal expansion coefficient and high plating adhesion. Furthermore, according to the present invention, there are provided a prepreg, a resin-coated film, a resin-coated metal foil, a metal-clad laminate, and a wiring board that can be obtained using the resin composition.

[0174] The present invention will be explained in more detail below with reference to examples, but the scope of the present invention is not limited to these examples.

[0175] [Examples 1 to 4, Comparative Examples 1 and 2] In these examples, each component used in preparing the resin composition will be described.

[0176] (Maleimide Compound (A)) Maleimide Compound-1: A maleimide compound (maleimide compound represented by the above formula (7)) synthesized as follows.

[0177] First, 48.5 g (0.4 mol) of 2,6-dimethylaniline, 272.0 g (1.4 mol) of α,α'-dihydroxy-1,3-diisopropylbenzene, 280 g of xylene, and 70 g of activated clay were charged into a 1 L flask equipped with a thermometer, a condenser, a Dean-Stark tube, and a stirrer, and the mixture was heated to 120 °C with stirring. Furthermore, the temperature was raised to 210 °C while removing the distillate water using a Dean-Stark tube. This allowed for a reaction for 6 hours. The mixture was then cooled to 140 °C, and 145.4 g (1.2 mol) of 2,6-dimethylaniline was charged, followed by heating to 220 °C. This allowed for a reaction for 3 hours. After the reaction, the mixture was air-cooled to 100 °C, diluted with 300 g of toluene, and the activated clay was removed by filtration. Low-molecular-weight substances such as the solvent and unreacted materials were distilled off under reduced pressure, yielding 345.2 g of a solid. The obtained solid was an amine compound represented by the following formula (29) (amine equivalent: 348, softening point: 71° C.).

[0178] In formula (29), n represents 0.95 to 10.

[0179] Next, 131.8 g (1.3 mol) of maleic anhydride and 700 g of toluene were charged into a 2 L flask equipped with a thermometer, a condenser, a Dean-Stark tube, and a stirrer, and the mixture was stirred at room temperature. Subsequently, a mixed solution of 345.2 g of the amine compound represented by formula (29) and 175 g of DMF was added dropwise over 1 hour. After the completion of the dropwise addition, the mixture was stirred at room temperature for an additional 2 hours to allow the reaction to proceed. Subsequently, 37.1 g of p-toluenesulfonic acid monohydrate was added, and the reaction solution was heated under reflux. The azeotropic water and toluene were cooled and separated, and then only the toluene was returned to the system, allowing the dehydration reaction to proceed for 8 hours. After air-cooling to room temperature, the mixture was concentrated under reduced pressure, and the brown solution was dissolved in 600 g of ethyl acetate. The solution was washed three times with 150 g of ion-exchanged water and three times with 150 g of a 2% aqueous sodium bicarbonate solution, dried over sodium sulfate, and then concentrated under reduced pressure. The resulting reaction product was vacuum-dried at 80°C for 4 hours, yielding 407.6 g of a solid. The obtained solid was analyzed by FD-MS spectrum, GPC, etc., and was found to be a maleimide compound represented by the formula (7) (a maleimide compound in which the amine of the amine compound represented by the formula (29) was modified to a maleimide, benzene ring equivalent: 153 g / mol, maleimide equivalent: 428 g / mol).

[0180] (Benzoxazine Compound (B)) Benzoxazine compound: a benzoxazine compound having an allyl group in the molecule (represented by the formula (5) above, R 3 and R 4 is an allyl group, X is a methylene group, and q and r are 1, and ALPd manufactured by Shikoku Chemicals Corporation

[0181] (Styrene-based polymer (C)) Styrene-based polymer: hydrogenated styrene (ethylene / butylene) styrene block copolymer (Tuftec H1041 manufactured by Asahi Kasei Corporation, weight average molecular weight Mw 80,000, solid at 25°C)

[0182] (Maleimide (D)) Maleimide compound-2: A maleimide compound not having an indane structure in the molecule (3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, BMI-5100 manufactured by Daiwa Chemical Industry Co., Ltd.) Maleimide compound-3: A maleimide compound not having an indane structure in the molecule (phenylmethane maleimide, BMI-2300 manufactured by Daiwa Chemical Industry Co., Ltd.)

[0183] (Reaction initiator) PBP: α,α'-di(t-butylperoxy)diisopropylbenzene (Perbutyl P (PBP) manufactured by NOF Corporation)

[0184] (Inorganic filler) Silica: silica particles surface-treated with a silane coupling agent having a phenylamino group in the molecule (SC2500-SXJ manufactured by Admatechs Co., Ltd.) Zinc molybdate: Z4SX-A1 manufactured by Admatechs Co., Ltd.

[0185] [Preparation Method] First, each component other than the inorganic filler was added to toluene and mixed to a solids concentration of 35% by mass in the composition (parts by mass) shown in Table 1. The mixture was stirred for 60 minutes. Thereafter, the inorganic filler was added to the resulting liquid, and the inorganic filler was dispersed using a bead mill. This resulted in a varnish-like resin composition (varnish).

[0186] Next, the resulting varnish was impregnated into glass cloth (#2118 type, T-glass, manufactured by Nitto Boseki Co., Ltd.) and then heated and dried at 130°C for about 3 minutes to obtain a prepreg. The thickness of the prepreg after curing was adjusted to about 104 µm (the content of organic components in the resin composition was about 44% by mass).

[0187] (Evaluation Board) Then, 12 sheets of each obtained prepreg were stacked, and 12 μm thick copper foil (3EC-VLP manufactured by Mitsui Mining & Smelting Co., Ltd.) was placed on both sides to form a pressure body, and heated and pressed at a temperature of 220° C. for 2 hours at a pressure of 3 MPa to obtain a copper foil-clad laminate (metal-clad laminate) with a thickness of approximately 1.25 mm, with copper foil bonded to both sides. This obtained copper foil-clad laminate was used as an evaluation board.

[0188] The evaluation substrate prepared as described above was evaluated by the following method.

[0189] [Dielectric Properties (Dielectric Constant Dk and Dielectric Loss Tangent Df)] The copper foil was removed from the evaluation board by etching. The resulting board was used as a test piece, and the dielectric constant and dielectric loss tangent at 10 GHz were measured using a cavity resonator perturbation method. Specifically, the dielectric constant (Dk) and dielectric loss tangent (Df) of the test piece at 10 GHz were measured using a network analyzer (N5230A manufactured by Keysight Technologies, Inc.). If the measured dielectric loss tangent was less than 0.0070, it was determined to be "passed."

[0190] [Thermal Expansion Coefficient] The copper foil was removed from the evaluation substrate by etching to obtain an unclad plate, which was used as a test specimen. The thermal expansion coefficient (CTE: ppm / °C) in the Y-axis direction was measured by the TMA method (Thermo-mechanical analysis) in accordance with IPC TM-650. A TMA device (TMA6000 manufactured by SII NanoTechnology Inc.) was used for the measurement, and measurements were made in the range of 50 to 260°C. If the measured thermal expansion coefficient was less than 5.5 ppm / °C, it was judged to be "passed."

[0191] [Glass Transition Temperature (Tg)] An unclad plate obtained by etching the copper foil off the evaluation substrate was used as a test specimen, and the Tg of the cured resin composition was measured using a Seiko Instruments Inc. viscoelasticity spectrometer "DMS6100." Dynamic mechanical analysis (DMA) was performed using a tensile module at a frequency of 10 Hz, and the temperature at which tan δ was maximized when the temperature was raised from room temperature to 340°C at a heating rate of 5°C / min was taken as Tg (°C). If the measured glass transition temperature was above 220°C, it was judged to be "passed." If the glass transition temperature Tg was above 310°C, it was indicated as ">310" in Table 1.

[0192] [Desmear Etching Rate] First, the copper foil on the surface of the evaluation substrate (copper foil-clad laminate) was removed by etching. In the desmear process, the substrate from which the copper foil had been removed was immersed in a swelling liquid (Swelling Dip Securigant P manufactured by Atotech Japan Co., Ltd.) at 60°C for 5 minutes, and then immersed in a potassium permanganate aqueous solution (Concentrate Compact CP manufactured by Atotech Japan Co., Ltd.) at 80°C for 10 minutes, followed by a neutralization treatment. This desmear process was carried out twice, and the weight of the substrate was measured before and after the desmear process was carried out twice. The weight loss due to the desmear process (weight of the substrate before the desmear process - weight of the substrate after two desmear processes) was calculated, and further, from this weight loss, a 1 mm 2 Weight loss per unit (mg / mm 2 ) was calculated. 2 The evaluation was made based on the weight loss per unit as follows:

[0193] 1 mm 2 The weight loss per 2 25mg / mm or more 2 If the weight loss (desmear etching rate) was within the above range, it was determined to be "pass." If the weight loss (desmear etching rate) was within the above range, it was found that the desmear property was excellent.

[0194] [Plating Adhesion] First, the copper foil on the surface of the evaluation substrate (copper foil-clad laminate) was removed by etching. Then, the same desmearing process as described in the desmear etch rate evaluation was performed (the desmearing process was performed twice). Subsequently, electroless copper plating and electrolytic copper plating were performed to a copper thickness of 30 μm. After annealing the evaluation substrate at 200° C. for 20 minutes, the copper was peeled from the evaluation substrate, and the peel strength at this time was measured in accordance with JIS C 6481 (1996). Specifically, a pattern measuring 10 mm in width and 80 mm in length was formed on the evaluation substrate, and the copper foil was peeled at a rate of 50 mm / min using a tensile tester, and the peel strength (N / mm) at this time was measured. This peel strength is the plating peel strength (plating adhesion). It can be seen that the higher this peel strength is, the better the adhesion to the plating. A plating peel strength of more than 0.4 N / mm was judged to be "pass."

[0195] [Copper Foil Peel Strength] The metal foil (copper foil) was peeled from the evaluation substrate (metal-clad laminate), and the peel strength at this time was measured in accordance with JIS C 6481 (1996). Specifically, a pattern 10 mm wide and 100 mm long was formed on the evaluation substrate, and the copper foil was peeled at a rate of 50 mm / min using a tensile tester, and the peel strength (N / mm) at this time was measured. This peel strength is the copper foil peel strength. The higher this peel strength, the higher the adhesion of the metal foil (copper foil). If the measured copper foil peel strength was more than 0.5 N / mm, it was judged to be "passed."

[0196] [Interlayer Peel Strength] The uppermost insulating layer (prepreg) was peeled off from the evaluation substrate (metal-clad laminate) at a rate of 50 mm / min using a tensile tester (i.e., the uppermost insulating layer was peeled off from the insulating layer underneath), and the peel strength (N / mm) at this time was measured. This peel strength is the interlayer peel strength. It was found that the higher this peel strength, the higher the interlayer adhesion, and if the measured interlayer peel strength was more than 0.5 N / mm, it was judged to be "passed."

[0197] The results of the above evaluations are shown in Table 1.

[0198] As can be seen from Table 1, when resin compositions (Examples 1 to 4) containing a maleimide compound (A) having an indane structure represented by formula (1) in its molecule, a benzoxazine compound (B) having an allyl group in its molecule, and a styrene-based polymer (C) that is solid at 25°C were used, the thermal expansion coefficient was lower and plating adhesion was higher than when those compositions (Comparative Examples 1 and 2) did not contain the maleimide compound (A), the thermal expansion coefficient was lower than when those compositions (Comparative Example 1) did not contain the styrene-based polymer (C). Furthermore, when the resin compositions of Examples 1 to 4 were used, not only was the thermal expansion coefficient lower but plating adhesion was also higher than when those compositions (Comparative Example 2) contained a maleimide compound other than the maleimide compound (A) having an indane structure represented by formula (1) in its molecule. Furthermore, it was found that when the resin compositions according to Examples 1 to 4 were used, cured products could be obtained that not only had a low thermal expansion coefficient and high plating adhesion, but also had a low dielectric tangent, a high glass transition temperature, and excellent adhesion to metal foil, interlayer adhesion, and desmear properties.

[0199] This application is based on Japanese Patent Application No. 2023-056557 filed on March 30, 2023, the contents of which are incorporated herein by reference.

[0200] In order to express the present invention, the present invention has been properly and sufficiently described through the embodiments in the above, but it should be recognized that those skilled in the art can easily change and / or improve the above-mentioned embodiments. Therefore, unless the changes or improvements made by those skilled in the art are at a level that causes departure from the scope of the claims described in the claims, such changes or improvements are interpreted as being included in the scope of the claims.

[0201] The present invention provides a resin composition that can give a cured product having a low thermal expansion coefficient and high plating adhesion. The present invention also provides a prepreg, a resin-coated film, a resin-coated metal foil, a metal-clad laminate, and a wiring board that can be obtained using the resin composition.

Claims

1. A resin composition comprising: a maleimide compound (A) having an indane structure represented by the following formula (1) in the molecule; a benzoxazine compound (B) having an allyl group in the molecule; and a styrene-based polymer (C) that is solid at 25°C. [In formula (1), each Rb independently represents an alkyl group having 1 to 10 carbon atoms, an alkyloxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a nitro group, a hydroxyl group, or a mercapto group, and r represents 0 to 3.] 2. The resin composition according to claim 1, wherein the maleimide compound (A) comprises a maleimide compound (A1) represented by the following formula (2): [In formula (2), each Ra is independently an alkyl group having 1 to 10 carbon atoms, an alkyloxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a nitro group, a hydroxyl group, or a mercapto group; each Rb is independently an alkyl group having 1 to 10 carbon atoms, an alkyloxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a nitro group, a hydroxyl group, or a mercapto group; q is 0 to 4, r is 0 to 3, and n is 0.95 to 10.] 3. The resin composition according to claim 1, wherein the benzoxazine compound (B) comprises at least one selected from the group consisting of a benzoxazine compound (B1) having a benzoxazine group represented by the following formula (3) in the molecule, a benzoxazine compound (B2) having a benzoxazine group represented by the following formula (4) in the molecule, and a benzoxazine compound (B3) having a benzoxazine group represented by the following formula (3) and a benzoxazine group represented by the following formula (4) in the molecule. [In formula (3), R 1 represents an allyl group, and p represents 1 to 4. [In formula (4), R 2 represents an allyl group.

4. The resin composition according to claim 3, wherein the benzoxazine compound (B1) includes a benzoxazine compound (B4) represented by the following formula (5): [In formula (5), R 3 and R 4 represents an allyl group, X represents an ether bond or an alkylene group, and q and r each independently represent an integer from 1 to 4.

5. The resin composition according to claim 1, wherein the styrene-based polymer (C) comprises at least one selected from the group consisting of methylstyrene (ethylene / butylene)-methylstyrene block copolymer, methylstyrene (ethylene-ethylene / propylene)-methylstyrene block copolymer, styrene-isoprene block copolymer, styrene-isoprene-styrene block copolymer, styrene (ethylene / butylene)-styrene block copolymer, styrene (ethylene-ethylene / propylene)-styrene block copolymer, styrene-butadiene block copolymer, styrene-isobutylene-styrene block copolymer, styrene (butadiene / butylene)-styrene block copolymer, and hydrogenated products of at least a portion of these.

6. The resin composition according to claim 1, wherein the styrene polymer (C) is at least partially hydrogenated.

7. The resin composition according to claim 1, further comprising an organic component other than the maleimide compound (A), the benzoxazine compound (B), and the styrene-based polymer (C), wherein the organic component includes at least one selected from the group consisting of a maleimide compound (D) different from the maleimide compound (A), a benzoxazine compound (E) different from the benzoxazine compound (B), an epoxy compound, a methacrylate compound, an acrylate compound, a vinyl compound, a cyanate ester compound, an active ester compound, and an allyl compound.

8. The resin composition according to claim 1, wherein the content of the maleimide compound (A) is 30 to 80 parts by mass per 100 parts by mass of the maleimide compound (A) and the benzoxazine compound (B) combined.

9. The resin composition according to claim 1, wherein the content of the maleimide compound (A) is 20 to 60 parts by mass per 100 parts by mass of the total of the maleimide compound (A), the benzoxazine compound (B), and the styrene-based polymer (C).

10. The resin composition according to claim 1, wherein the content of the styrene-based polymer (C) is 15 to 40 parts by mass per 100 parts by mass of the total of the maleimide compound (A), the benzoxazine compound (B), and the styrene-based polymer (C).

11. The resin composition according to claim 1, further comprising an inorganic filler.

12. The resin composition according to claim 11, wherein the content of the inorganic filler is 50 to 250 parts by mass per 100 parts by mass of the total of the maleimide compound (A), the benzoxazine compound (B), and the styrene-based polymer (C).

13. A prepreg comprising the resin composition according to any one of claims 1 to 12 or a semi-cured product of said resin composition and a fibrous base material.

14. A resin-coated film comprising a resin layer containing the resin composition according to any one of claims 1 to 12 or a semi-cured product of said resin composition, and a support film.

15. A resin-coated metal foil comprising a resin layer containing the resin composition according to any one of claims 1 to 12 or a semi-cured product of said resin composition, and a metal foil.

16. A metal-clad laminate comprising an insulating layer containing a cured product of the resin composition according to any one of claims 1 to 12, and a metal foil.

17. A metal-clad laminate comprising an insulating layer containing the cured product of the prepreg according to claim 13 and a metal foil.

18. A wiring board comprising an insulating layer containing a cured product of the resin composition according to any one of claims 1 to 12, and wiring.

19. A wiring board comprising an insulating layer containing the cured product of the prepreg according to claim 13 and wiring.

Citation Information

Patent Citations

  • Resin composition and prepreg, laminated board and printed circuit board using same

    CN113121999A

  • Resin composition, cured product of resin composition, resin sheet, printed wiring board and semiconductor device

    JP2020158705A

  • Resin sheet

    JP2022146808A

  • Resin composition, prepreg, film provided with resin, metal foil provided with resin, metal-clad laminate, and wiring board

    WO2022054864A1