Photosensitive composition, pattern-forming method using same, and transition metal cluster compound

A photosensitive composition with a transition metal cluster compound addresses the resolution and sensitivity challenges in semiconductor photolithography, enabling the formation of ultra-fine patterns with high resolution and low roughness, facilitating further circuit miniaturization.

WO2024202889A1PCT designated stage expired Publication Date: 2024-10-03MITSUBISHI CHEM CORP +1

Patent Information

Application Number
PCT/JP2024/007487
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-02-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional chemically amplified photoresists used in semiconductor photolithography face challenges in achieving high resolution and low roughness for ultra-fine patterns due to acid diffusion, limiting further miniaturization of circuit patterns.

Method used

A photosensitive composition containing a transition metal cluster compound with a specific structure, capable of forming clusters centered on metal elements and incorporating ligands, oxygen, and hydroxyl groups, is developed, which is highly sensitive to actinic radiation and suitable for forming ultra-fine patterns.

Benefits of technology

The photosensitive composition achieves high resolution and sensitivity, enabling the formation of fine patterns with half pitch as low as 50 nm, surpassing the limitations of conventional resists in circuit miniaturization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024007487_03102024_PF_FP_ABST
    Figure JP2024007487_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a photosensitive composition containing a metal cluster compound capable of realizing miniaturization of circuit patterns. The present invention pertains to a photosensitive composition containing a metal cluster compound that forms a cluster having a metal element at the center, that is formed from the metal element and a ligand represented by general formula (1), and that optionally contains oxygen and / or a hydroxyl group. (In formula (1), X1 and X2 each independently represent a halogen atom, and may be identical or different, and R1, R2, and R3 each independently represent hydrogen or an arbitrarily-defined substituent, and may be identical or different.)
Need to check novelty before this filing date? Find Prior Art

Description

Photosensitive composition, pattern formation method using same, and transition metal cluster compound

[0001] The present invention relates to a transition metal cluster compound suitable for use in ultra-microlithography processes such as the manufacture of VLSIs and high-capacity microchips, as well as other photofabrication processes, a photosensitive composition containing the same, and a pattern formation method using the photosensitive composition.

[0002] Traditionally, semiconductor device manufacturing processes involve fine processing using lithography with photoresist compositions. In semiconductor photolithography, circuit patterns become smaller as semiconductor devices become smaller, according to Moore's Law, and further miniaturization is desired. Photolithography is broadly based on the shortening of wavelengths of the light source used in exposure equipment and the photoresists that react to this wavelength. Photoresists are required to satisfy all of the following requirements: high resolution, low roughness, and high sensitivity. Conventional resists containing photoacid generators, known as chemically amplified resists, are thought to be unable to handle ultrafine patterns because acid diffusion leads to a decrease in resolution.

[0003] In recent years, non-chemically amplified photoresists based on compounds containing metal elements such as Zn and Sn have been proposed, and it has been reported that they can be used to form fine patterns using next-generation exposure equipment that uses extreme ultraviolet (EUV) light.

[0004] For example, Patent Documents 1 to 5 and Non-Patent Documents 1 to 3 listed below disclose methods of forming resist patterns using extreme ultraviolet rays (EUV light) or electron beams.

[0005] JP 2015-108781 A JP 2001-072716 A JP 2017-173537 A JP 2012-185484 A JP 2021-102604 A

[0006] Minoru Toriumi etc.,Proc.SPIE,9779(2016)97790GLianjia Wu etc.,Proc.SPIE,10957(2019)109570BNeha Thakur etc.,Proc.SPIE,10957(2019)10957D

[0007] In photolithography, particularly in semiconductor photolithography, there is a demand for photosensitive compositions and pattern formation methods that can realize even finer circuit patterns.

[0008] As a result of extensive research, the present inventors have found that metal cluster compounds having specific structures are suitable as photoresists for ultrafine patterns. Accordingly, an object of the present invention is to provide a photosensitive composition containing a transition metal cluster compound that can realize finer circuit patterns, a pattern formation method using this photosensitive composition, and a metal cluster compound suitable for the photosensitive composition.

[0009] The present invention has the following aspects.

[0010] [1] A photosensitive composition comprising a metal cluster compound, which is a compound forming a cluster centered on a metal element, and which is composed of the metal element and a ligand represented by the following general formula (1), and which optionally contains oxygen and / or a hydroxyl group within the structure:

[0011] (In the above formula (1), X 1 and X 2 are each independently a halogen atom and may be the same or different, R 1 , R 2 , R 3 are each independently hydrogen or any substituent, and may be the same or different.

[0012] [2] The photosensitive composition according to [1], wherein the ligand is a ligand represented by the following general formula (2):

[0013] (In the above formula (2), X 1 and X 2 are each independently a halogen atom and may be the same or different, R 1 , R 3 , R 4 are each independently hydrogen or any substituent, and may be the same or different.

[0014] [3] The photosensitive composition according to [1] or [2], wherein the number of metal elements in the metal cluster compound is 2 to 12.

[0015] [4] The photosensitive composition according to any one of [1] to [3], wherein the number of metal elements in the metal cluster compound is a number that results in electrical neutrality.

[0016] [5] The photosensitive composition according to any one of [1] to [4], wherein the metal element is bismuth.

[0017] [6] X in the formula (1) or the formula (2) 1 and X 2 and are both chlorine.

[0018] [7] R in the formula (1) or the formula (2) 1 , R 3 and are both hydrogen.

[0019] [8] R in the formula (2) 4 The photosensitive composition according to any one of [2] to [7], wherein the hydrocarbon group has 1 to 20 carbon atoms.

[0020] [9] R in the formula (2) 4

[0022] The photosensitive composition according to any one of [2] to [8], wherein is a linear or branched saturated hydrocarbon group.

[0021]

[10] The photosensitive composition according to any one of [1] to [9], further comprising a photoacid generator that generates an acid under the action of actinic radiation.

[0022]

[11] The photosensitive composition according to any one of [1] to

[10] , wherein the molecular weight of the metal cluster compound is 300 to 8,000.

[0023]

[12] The photosensitive composition according to any one of [1] to

[11] , further comprising an organic solvent.

[0024]

[13] The photosensitive composition according to any one of [1] to

[12] , wherein the content of the metal cluster compound is 1 to 30 mass %.

[0025]

[14] The photosensitive composition according to

[10] , wherein the actinic radiation has a wavelength of 6.5 to 13.5 nm.

[0026]

[15] A pattern forming method, comprising a step of forming a photosensitive layer on a substrate by spin coating using the photosensitive composition according to any one of [1] to

[14] .

[0027]

[16] A pattern formation method comprising: a step of forming a photosensitive layer on a substrate using the photosensitive composition according to any one of [1] to

[14] ; a step of irradiating predetermined regions of the photosensitive layer with actinic radiation to perform pattern exposure; and a step of developing the exposed photosensitive layer with a developer to selectively remove exposed or unexposed regions of the photosensitive layer.

[0028]

[17] The pattern formation method according to

[15] , wherein the developer is an organic solvent having a solubility parameter (SP value) of 7.5 to 11.

[0029]

[18] A metal cluster compound which is a compound forming a cluster centered on a metal element and is composed of 2 to 12 metal elements and a ligand represented by the following general formula (2):

[0030] (In the above formula (2), X 1 and X 2 are each independently a halogen atom and may be the same or different, R 1 , R 3 , R 4 are each independently hydrogen or any substituent, and may be the same or different.

[0031]

[19] The metal cluster compound according to

[18] , wherein the number of metal elements in the metal cluster compound is 2 to 12.

[0032]

[20] The metal cluster compound according to

[18] or

[19] , wherein the metal element is bismuth.

[0033]

[21] X in the formula (2) 1 and X 2 and each represent chlorine.

[0034]

[22] R in the formula (2) 1 , R 3 and are both hydrogen.

[18] The metal cluster compound according to any one of

[18] to

[21] .

[0035]

[23] R in the formula (2) 4 The metal cluster compound according to any one of

[18] to

[22] , wherein the hydrocarbon group has 1 to 20 carbon atoms.

[0036]

[24] R in the formula (2) 4 The metal cluster compound according to any one of

[18] to

[23] , wherein is a linear or branched saturated hydrocarbon group.

[0037] The photosensitive composition of the present invention is highly sensitive to actinic radiation exposure, and can form, for example, an L&S (line and space) 1:1 pattern with a half pitch (hp) of 100 nm or 50 nm in an electron beam (EB) lithography test, thereby achieving high resolution.

[0038] The present invention will be described below based on one embodiment. However, the present invention is not limited to this embodiment. Note that, although the present specification uses "to" to express a numerical range from a lower limit value to an upper limit value, the numerical range in this description is a numerical range specified as being equal to or greater than the lower limit value and equal to or less than the upper limit value, including the lower limit value and the upper limit value.

[0039] [Photosensitive Composition] A photosensitive composition according to one embodiment of the present invention (hereinafter also referred to as the present photosensitive composition) contains a metal cluster compound (hereinafter also referred to as the present cluster compound) composed of a metal element and a ligand represented by the following general formula (1): In the present invention, a cluster compound refers to a compound having a metal atom and a ligand, forming a cluster centered around the metal atom, and is a metal complex molecule in which multiple metal atoms are bonded to each other directly or through a bridging ligand. The present cluster compound may contain oxygen and / or hydroxyl groups within its structure, preferably a μ-oxo ligand (μ-O) and / or a μ-hydroxy group (μ-OH).

[0040] (In the above formula (1), X 1 and X 2 are each independently a halogen atom and may be the same or different, R 1 , R 2 , R 3 are each independently hydrogen or any substituent, and may be the same or different.

[0041] [Cluster Compound of the Present] Metals in the cluster compound of the present invention include transition metals and non-transition metals. Examples of transition metal elements include zinc, cadmium, gold, silver, copper, platinum, palladium, nickel, iridium, rhodium, cobalt, osmium, ruthenium, iron, rhenium, manganese, tungsten, molybdenum, chromium, tantalum, zirconium, titanium, yttrium, and scandium. Examples of non-transition metals include aluminum, gallium, indium, thallium, tin, lead, bismuth, and antimony. The metal in the cluster compound of the present invention is preferably one or more selected from these metals, and among these, non-transition metals are preferred, with bismuth being particularly preferred from the viewpoints of high absorption of ionizing radiation and safety.

[0042] In some cases, it may not be possible to clearly distinguish whether the cluster compound has a single cluster structure or a mixture of cluster structures with different numbers of metal elements. However, even in such cases, in order to increase the solubility of the cluster compound in a solvent, the number of metal elements is preferably two or more, more preferably three or more. More specifically, the number of metal elements is preferably in the range of 2 to 12, 2 to 6, 4 to 6, or 5 to 6, with six being particularly preferred. In the case of a mixture, the cluster compound preferably has the most cluster structural components with six metal elements. The cluster compound is preferably electrically neutral, and the number of metal elements is preferably set to be such that it is electrically neutral. In other words, the metal complex compound and the cluster compound are preferably not cationic or anionic.

[0043] In the above general formula (1), X 1 and X 2are each independently a halogen atom, and may be the same or different. More specifically, they are fluorine, chlorine, bromine, etc., and X 1 and X 2 Preferably, one or both of the groups is chlorine.

[0044] In the above general formula (1), R 1 , R 2 , R 3 are hydrogen or any substituent, which may be the same or different. The optional substituent may include a hydrocarbon group. The hydrocarbon group may contain double bonds, aromatic groups, or different elements such as oxygen, sulfur, or nitrogen. 1 When R is a hydrocarbon group, the number of carbon atoms is preferably 0 to 20, more preferably 0 to 10. 2 When R is a hydrocarbon group, the number of carbon atoms is preferably 0 to 20, more preferably 0 to 10. 3 When the hydrocarbon group is a hydrocarbon group, it preferably has 0 to 20 carbon atoms, more preferably 0 to 10 carbon atoms.

[0045] R 1 , R 2 , R 3More specifically, examples of the alkyl group include hydrogen, alkyl groups such as a methyl group, an ethyl group, a propyl group, and a 2-ethylhexyl group, alkoxy groups such as a methoxy group, an ethoxy group, a propoxy group, and a 2-ethylhexyloxy group, alkyl ester groups such as a methyl ester group, an ethyl ester group, a propyl ester group, and a 2-ethylhexyl ester group, alkylcarbamoyl groups such as a methylcarbamoyl group, an ethylcarbamoyl group, a propylcarbamoyl group, and a 2-ethylhexylcarbamoyl group, alkylcarbamic acid ester groups such as a methylcarbamic acid ester group, an ethylcarbamic acid ester, a propylcarbamic acid ester, and a 2-ethylhexylcarbamic acid ester group, alkylsulfonic acid ester groups such as a methylsulfonic acid ester group, an ethylsulfonic acid ester group, a propylsulfonic acid ester group, and a 2-ethylhexylsulfonic acid ester group, and alkylphosphonic acid ester groups such as a methylphosphonic acid ester group, an ethylphosphonic acid ester group, a propylphosphonic acid ester group, and a 2-ethylhexylphosphonic acid ester group. Among these, R 1 , R 3 is preferably hydrogen, and R 2 is preferably an alkyl ester group such as a methyl ester group, an ethyl ester group, a propyl ester group, or a 2-ethylhexyl ester group; an alkylcarbamoyl group such as a methylcarbamoyl group, an ethylcarbamoyl group, a propylcarbamoyl group, or a 2-ethylhexylcarbamoyl group; or an alkylcarbamate group such as a methylcarbamate group, an ethylcarbamate ester, a propylcarbamate ester, or a 2-ethylhexylcarbamate group.

[0046] A more specific structure of the above general formula (1) is, for example, the following general formula (2).

[0047] (In the above formula (2), X 1 and X 2 are each independently a halogen atom and may be the same or different, R 1 , R 3 , R 4are each independently hydrogen or any substituent, and may be the same or different.

[0048] In the above general formula (2), X 1 , X 2 , R 1 , R 3 is the same as in the above general formula (1).

[0049] In the above general formula (2), R 4 is hydrogen or an optional substituent. The optional substituent may be a hydrocarbon group. The hydrocarbon group may contain double bonds, aromatic groups, or different elements such as oxygen, sulfur, or nitrogen. 4 When the hydrocarbon group is a hydrocarbon group, it preferably has 1 to 20 carbon atoms, more preferably 1 to 10 carbon atoms.

[0050] R 4 More specifically, examples of the alkyl group include alkyl groups such as a methyl group, an ethyl group, a propyl group, and a 2-ethylhexyl group; alkoxy groups such as a methoxy group, an ethoxy group, a propoxy group, and a 2-ethylhexyloxy group; alkyl ester groups such as a methyl ester group, an ethyl ester group, a propyl ester group, and a 2-ethylhexyl ester group; alkylcarbamoyl groups such as a methylcarbamoyl group, an ethylcarbamoyl group, a propylcarbamoyl group, and a 2-ethylhexylcarbamoyl group; alkylcarbamic acid ester groups such as a methylcarbamic acid ester, an ethylcarbamic acid ester, a propylcarbamic acid ester, and a 2-ethylhexylcarbamic acid ester group; alkylsulfonic acid ester groups such as a methylsulfonic acid ester group, an ethylsulfonic acid ester group, a propylsulfonic acid ester group, and a 2-ethylhexylsulfonic acid ester group; and alkylphosphonic acid ester groups such as a methylphosphonic acid ester group, an ethylphosphonic acid ester group, a propylphosphonic acid ester group, and a 2-ethylhexylphosphonic acid ester group. Among these, R 4is preferably a linear or branched saturated hydrocarbon group, and examples thereof include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group, an isopropyl group, an isobutyl group, a tert-butyl group, an isopentyl group, and a 2-ethylhexyl group.

[0051] The molecular weight of the cluster compound is preferably 300 to 50,000, more preferably 1,000 to 10,000, and even more preferably 2,000 to 8,000. If the molecular weight of the cluster compound is below the upper limit, the volume is small, and therefore roughness and resolution are expected to be improved. On the other hand, if the molecular weight is above the lower limit, coating properties and etching resistance tend to be improved. Note that this molecular weight is a guideline, and is not intended to be limiting, as it does not determine lithography properties by itself.

[0052] [Method for Producing the Present Cluster Compound] The present cluster compound can be produced, for example, by reacting a phenyl compound of a metal element with a phenol derivative having a protonated structure represented by the general formula (1) or (2). More specifically, the phenyl compound of a metal element and the phenol derivative having a protonated structure represented by the general formula (1) or (2) are placed in a reaction vessel and refluxed in toluene for an extended period of time. The reflux stirring time is preferably 1 to 48 hours, more preferably 10 to 48 hours. After reflux stirring, a small amount of water is added, followed by stirring for approximately 10 minutes, vacuum concentration, and purification of the residue by silica gel column chromatography or the like to obtain the present cluster compound. The reaction temperature is preferably room temperature, specifically 15 to 40°C, more preferably 20 to 30°C. A sealed reaction vessel is preferred; for small volumes, a Schlenk tube or the like can be used. The reaction is preferably carried out under an argon atmosphere.

[0053] An example of the phenyl compound of a metal element is triphenylbismuth.

[0054] Examples of the phenol derivative having a structure in which a proton is added to the structure represented by the general formula (1) include X 1 and X 2 is a chlorine atom, R 1 and R 3 is a hydrogen atom, R 2 is a methyl group, and the like. Examples of phenol derivatives having a structure in which a proton is added to the structure represented by the general formula (2) include, for example, 2,6-dichloro-4-methylphenol, 1 and X 2 is a chlorine atom, R 1 and R 3 is a hydrogen atom, R 4 When is a methyl group, examples include methyl(3,5-dichloro-4-hydroxyphenyl)carbamate.

[0055] The phenyl compound of a metal element and the phenol derivative having a structure in which a proton is added to the structure represented by the general formula (1) are mixed preferably in a weight ratio of 1:2 to 1:10, more preferably 1:3 to 1:5.

[0056] [Photosensitive Composition of the Present] The photosensitive composition of the present invention contains the present cluster compound. The photosensitive composition of the present invention may contain only one type of the present cluster compound, or may contain two or more types of the present cluster compound.

[0057] The content of the present cluster compound in the present photosensitive composition is usually 30 to 100% by mass, preferably 40 to 100% by mass, and particularly preferably 50 to 100% by mass, based on the total of all components of the photosensitive composition other than the solvent. When the present cluster compound is used as a photosensitizer in the photosensitive composition, the content of the present cluster compound is usually 1 to 30% by mass, preferably 1 to 20% by mass, and particularly preferably 1 to 10% by mass, based on the photosensitive composition. When the content of the present cluster compound in the present photosensitive composition is equal to or greater than the above-mentioned lower limit, good exposure sensitivity can be obtained.

[0058] [Photoacid Generator] The photosensitive composition can also function by containing, together with the cluster compound, a photoacid generator that generates an acid when exposed to actinic radiation. Examples of actinic radiation include the bright line spectrum of a mercury lamp, far ultraviolet radiation represented by an excimer laser, extreme ultraviolet radiation (EUV light), X-rays, and electron beams (EB). From the viewpoint of resolution, however, exposure wavelengths that are shorter are preferred, such as extreme ultraviolet radiation (EUV light) or electron beams (EB) that emit light with a wavelength of 6.5 nm to 13.5 nm.

[0059] The photoacid generator that generates an acid when exposed to actinic radiation is not particularly limited as long as it is a known compound, but is preferably a compound that generates an organic acid, such as at least one of sulfonic acid, bis(alkylsulfonyl)imide, and tris(alkylsulfonyl)methide, when exposed to actinic radiation.

[0060] The photoacid generators can be used alone or in combination of two or more. When two or more types are used in combination, preferred embodiments include (1) the use of two photoacid generators with different acid strengths, and (2) the use of two photoacid generators with different sizes (molecular weights or carbon numbers) of the acids they generate. Examples of the embodiment (1) include the use of a fluorine-containing sulfonic acid generator and a tris(fluoroalkylsulfonyl)methide acid generator, a fluorine-containing sulfonic acid generator and a non-fluorine-containing sulfonic acid generator, and an alkylsulfonic acid generator and an arylsulfonic acid generator. Examples of the embodiment (2) include the use of two photoacid generators whose acid anions differ in the number of carbon atoms by four or more.

[0061] In particular, the present photosensitive composition is preferably a photosensitive composition for use with actinic radiation, and a photosensitive composition that reacts with actinic radiation is preferred because the development speed in a developer changes and a pattern can be formed after a certain period of development. As actinic radiation, a shorter wavelength of light is preferred because higher resolution can be obtained, and light with a wavelength of 6.5 nm to 13.5 nm, i.e., extreme ultraviolet light (EUV light) or an electron beam (EB), is preferred. That is, the present photosensitive composition is preferably a photosensitive composition that reacts with light or an electron beam with a wavelength of 6.5 nm to 13.5 nm.

[0062] The present photosensitive compound reacts with light even when used alone in a photosensitive composition. Addition of a photoacid generator synergistically enhances photosensitivity with the present cluster compound in the photosensitive composition, thereby enhancing the photosensitivity of the present cluster compound. Therefore, adding a photoacid generator is preferable when a photosensitive composition composed solely of the present cluster compound does not have sufficient photosensitivity for the required specifications. When the present photosensitive composition contains a photoacid generator, the content of the photoacid generator in the present photosensitive composition (the total amount when multiple photoacid generators are used) is preferably 0.1 to 30% by mass, more preferably 0.5 to 20% by mass, and even more preferably 1 to 15% by mass, based on the total components of the photosensitive composition other than the solvent. When the content of the photoacid generator in the photosensitive composition is equal to or greater than the lower limit, the photosensitivity is enhanced. When the content is equal to or less than the upper limit, the composition is less susceptible to the poor film-forming properties of the photoacid generator, thereby achieving good film-forming properties based on the present photosensitive compound.

[0063] [Solvent] The present photosensitive composition usually contains a solvent for preparing the composition, and this solvent is preferably an organic solvent. The solvent for preparing the photosensitive composition is not particularly limited as long as it dissolves each component, and examples thereof include alkylene glycol monoalkyl ether carboxylates (such as propylene glycol monomethyl ether acetate (PGMEA; 1-methoxy-2-acetoxypropane)), alkylene glycol monoalkyl ethers (such as propylene glycol monomethyl ether (PGME; 1-methoxy-2-propanol)), alkyl lactate esters (such as ethyl lactate and methyl lactate), cyclic lactones (such as γ-butyrolactone, preferably having 4 to 10 carbon atoms), linear or cyclic ketones (such as 2-heptanone and cyclohexanone, preferably having 4 to 10 carbon atoms), alkylene carbonates (such as ethylene carbonate and propylene carbonate), alkyl carboxylates (preferably alkyl acetates such as butyl acetate), alkyl alkoxyacetates (ethyl ethoxypropionate), alkylamides (N,N-dimethylformamide), and alkyl sulfoxides (dimethyl sulfoxide). Other usable solvents include, for example, the solvents described in paragraphs

[0244] and after of US Patent Application Publication No. 2008 / 0248425A1.

[0064] Of the above, N,N-dimethylformamide, dimethyl sulfoxide, alkylene glycol monoalkyl ether carboxylate and alkylene glycol monoalkyl ether are preferred.

[0065] These solvents may be used alone or in combination of two or more. When two or more solvents are mixed, it is preferable to mix a solvent having a hydroxyl group with a solvent not having a hydroxyl group. As the solvent having a hydroxyl group, alkylene glycol monoalkyl ether is preferred, and as the solvent not having a hydroxyl group, alkylene glycol monoalkyl ether carboxylate, N,N-dimethylformamide, and dimethyl sulfoxide are preferred.

[0066] The content of the solvent in the total amount of the photosensitive composition can be adjusted as appropriate depending on the film thickness of the pattern to be formed, etc., but is generally adjusted so that the total concentration of components other than the solvent in the photosensitive composition is 0.5 to 30 mass %, preferably 1.0 to 20 mass %, more preferably 1.5 to 10 mass %, and even more preferably 1.5 to 5 mass %.

[0067] [Surfactant] The photosensitive composition preferably further contains a surfactant. The surfactant is preferably a fluorine-based and / or silicone-based surfactant. Examples of such surfactants include Megafac F176 and Megafac R08 manufactured by Dainippon Ink and Chemicals, Inc., PF656 and PF6320 manufactured by OMNOVA, Troisol S-366 manufactured by Troy Chemical Co., Ltd., Fluorad FC430 manufactured by Sumitomo 3M Limited, and Polysiloxane Polymer KP-341 manufactured by Shin-Etsu Chemical Co., Ltd. Surfactants other than fluorine-based and / or silicone-based surfactants can also be used. More specifically, examples include polyoxyethylene alkyl ethers and polyoxyethylene alkyl aryl ethers.

[0068] Other known surfactants may also be used as appropriate, such as those described in U.S. Patent Application Publication No. 2008 / 0248425A1, paragraphs

[0273] and thereafter.

[0069] The surfactant may be used alone or in combination of two or more kinds. The content of the surfactant is preferably 0.0001 to 2 mass %, more preferably 0.001 to 1 mass %, based on the total mass of the components other than the solvent in the photosensitive composition.

[0070] [Resin] The photosensitive composition can be used alone to form a pattern, but it may also contain a resin material in addition to the cluster compound. Resin materials are not particularly limited as long as they are soluble in a solvent, and examples include novolac resins, styrene resins, and acrylic resins. They may be used alone or in combination of two or more types. Their molecular structure may contain dissolution-inhibiting groups that decompose in the presence of chemically active species such as acids or radicals, or crosslinking groups that crosslink, or they may be copolymer resins of two or more types. Examples of dissolution-inhibiting groups that decompose in the presence of chemically active species such as acids or radicals include alkoxycarbonyl groups and acetal groups. Examples of crosslinking groups that crosslink in the presence of chemically active species such as acids or radicals include vinyl groups, carbodiimide groups, N-hydroxyester groups, imide ester groups, maleimide groups, haloacetyl groups, pyridyl disulfide groups, hydrazide groups, alkoxyamino groups, and diazirine groups.

[0071] [Other Additives] In addition to the components described above, the photosensitive composition may contain, as appropriate, carboxylic acids, carboxylic acid onium salts, dissolution-inhibiting compounds with a molecular weight of 3,000 or less as described in, for example, Proceedings of SPIE, 2724, 355 (1996), dyes, plasticizers, photosensitizers, light absorbers, crosslinking agents, antioxidants, and the like. Carboxylic acids are particularly preferred for improving performance. Preferred carboxylic acids include aromatic carboxylic acids such as benzoic acid and naphthoic acid. The carboxylic acid content is preferably 0.01 to 10% by mass, more preferably 0.01 to 5% by mass, and even more preferably 0.01 to 3% by mass, based on the total weight of the components of the photosensitive composition other than the solvent.

[0072] [Method for Producing the Present Photosensitive Composition] The present photosensitive composition can be produced by dissolving the present cluster compound, a photoacid generator (if used) and other components in a solvent for preparation, and filtering the solution as needed. The filter is preferably made of polytetrafluoroethylene, polyethylene, or nylon with a pore size of 0.2 μm or less, more preferably 0.1 μm or less, and even more preferably 0.05 μm or less.

[0073] [Pattern Forming Method] A pattern forming method according to one embodiment of the present invention (hereinafter also referred to as the present pattern forming method) comprises the steps of forming a photosensitive layer on a substrate using the present photosensitive composition, irradiating predetermined regions of the photosensitive layer with actinic radiation to perform pattern exposure, and developing the exposed photosensitive layer with a developer to selectively remove exposed or unexposed regions of the photosensitive layer.

[0074] [Photosensitive Layer Formation Step] The photosensitive layer can be formed by applying the photosensitive composition to a substrate (e.g., silicon or silicon dioxide coated) such as those used in the manufacture of integrated circuit devices using a suitable coating method such as a spinner, followed by drying at 50 to 150°C. In this case, a commercially available inorganic or organic antireflective film can be used, if necessary. Furthermore, an antireflective film can be applied as an underlayer of the resist.

[0075] [Exposure Step] In the present invention, "exposure" refers to drawing by irradiation with actinic radiation. Unless otherwise specified, this term includes not only exposure with far ultraviolet light, X-rays, extreme ultraviolet light (EUV light), etc., as typified by mercury lamps and excimer lasers, but also drawing with particle beams such as electron beams and ion beams. Exposure can be performed, for example, by irradiating a formed photosensitive layer with high-energy radiation through a predetermined mask to predetermined regions to perform pattern exposure, or by irradiating with an electron beam to perform pattern exposure without using a mask (direct drawing). The actinic radiation is not particularly limited, but examples include KrF excimer lasers, ArF excimer lasers, extreme ultraviolet light (EUV light), and electron beams. Extreme ultraviolet light (EUV light) and electron beams (EB) are preferred. As described above, extreme ultraviolet light (EUV light) or electron beams (EB) emitting light with a wavelength of 6.5 nm to 13.5 nm are preferred.

[0076] After the exposure, baking (heating) may or may not be performed before development. When baking (heating) is performed, the heating temperature is preferably 50 to 150°C, more preferably 60 to 150°C, and even more preferably 80 to 140°C. When baking (heating) is performed, the heating time is preferably 30 to 300 seconds, more preferably 30 to 180 seconds, and even more preferably 30 to 90 seconds. Heating can be performed by means provided in a normal exposure / developing machine, and may be performed using a hot plate or the like.

[0077] [Developing Step] After the exposure, development is carried out using a developer to selectively remove the exposed or unexposed areas of the photosensitive layer.

[0078] [Developer] It is preferable to use an organic solvent as the developer, preferably an organic solvent having a vapor pressure of 5 kPa or less at 20° C., more preferably 3 kPa or less, and particularly preferably 2 kPa or less. By setting the vapor pressure of the organic solvent to 5 kPa or less, evaporation of the developer on the substrate or in the developing cup is suppressed, improving the temperature uniformity within the surface of the pattern-formed substrate, and as a result, improving the dimensional uniformity within the surface of the pattern-formed substrate.

[0079] The organic solvent used as the developer may be any of various organic solvents, including, for example, at least one solvent selected from ester solvents, ketone solvents, alcohol solvents, amide solvents, sulfoxide solvents, ether solvents, hydrocarbon solvents, etc. In particular, a developer containing at least one solvent selected from amide solvents, ketone solvents, ester solvents, alcohol solvents, and ether solvents is preferred.

[0080] Examples of ester-based solvents include alkyl carboxylate solvents such as methyl acetate, butyl acetate, ethyl acetate, isopropyl acetate, amyl acetate, ethyl-3-ethoxypropionate, propylene glycol diacetate, 3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, methyl formate, ethyl formate, butyl formate, propyl formate, ethyl lactate, butyl lactate, and propyl lactate; alkylene glycol monoalkyl ether carboxylate solvents such as propylene glycol monomethyl ether acetate (PGMEA; also known as 1-methoxy-2-acetoxypropane), ethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, and propylene glycol monoethyl ether acetate; and butyl acetate, amyl acetate, ethyl lactate, and propylene glycol monomethyl ether acetate are more preferred.

[0081] Examples of ketone solvents include 1-octanone, 2-octanone, 1-nonanone, 2-nonanone, acetone, 4-heptanone, 1-hexanone, 2-hexanone, diisobutyl ketone, cyclopentanone, cyclohexanone, methylcyclohexanone, phenylacetone, methyl ethyl ketone, methyl amyl ketone, methyl isobutyl ketone, acetylacetone, acetonylacetone, ionone, diacetonyl alcohol, acetylcarbinol, acetophenone, methyl naphthyl ketone, isophorone, and propylene carbonate. Alkyl ketone solvents, such as methyl isobutyl ketone, methyl amyl ketone, cyclopentanone, and cyclohexanone, are more preferred.

[0082] Examples of alcohol-based solvents include alcohols such as methyl alcohol, ethyl alcohol, n-propyl alcohol including 1-propanol or 2-propanol, isopropyl alcohol, n-butyl alcohol, sec-butyl alcohol, tert-butyl alcohol, isobutyl alcohol, hexyl alcohols such as n-hexyl alcohol, heptyl alcohols such as n-heptyl alcohol, octyl alcohols such as n-octyl alcohol, and decanols such as n-decanol; and glycols such as ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, and 1,4-butylene glycol. Examples of such solvents include glycerol-based solvents, alkylene glycol monoalkyl ether-based solvents such as ethylene glycol monomethyl ether, propylene glycol monomethyl ether (PGME; also known as 1-methoxy-2-propanol), ethylene glycol monoethyl ether, propylene glycol monoethyl ether, diethylene glycol monomethyl ether, and triethylene glycol monoethyl ether, glycol ether-based solvents such as methoxymethylbutanol and propylene glycol dimethyl ether, and phenol-based solvents such as phenol and cresol, with 1-hexanol, 2-hexanol, 1-octanol, 2-ethyl-hexanol, propylene glycol monomethyl ether, and cresol being more preferred.

[0083] Examples of the amide solvent that can be used include N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, hexamethylphosphoric triamide, 1,3-dimethyl-2-imidazolidinone, etc. Examples of the sulfoxide solvent that can be used include dimethyl sulfoxide, etc.

[0084] Examples of the ether solvent include the alkylene glycol monoalkyl ether solvents and glycol ether solvents described above, as well as dioxane, tetrahydrofuran, tetrahydropyran, and the like.

[0085] Examples of hydrocarbon solvents include aromatic hydrocarbon solvents such as toluene and xylene, and aliphatic hydrocarbon solvents such as pentane, hexane, octane, decane, and dodecane.

[0086] The developer preferably contains one or more solvents selected from alkylene glycol monoalkyl ether carboxylate solvents, alkylene glycol monoalkyl ether solvents, alkyl carboxylate solvents, and alkyl ketone solvents, and more preferably contains one or more solvents selected from dimethylformamide, dimethyl sulfoxide, tetrahydrofuran, ethylene glycol, methyl alcohol, ethyl alcohol, 1-propanol, and 2-propanol.

[0087] As the developer, it is preferable to use a developer containing at least one organic solvent selected from the group consisting of ester solvents having no hydroxyl group in the molecule, ketone solvents having no hydroxyl group in the molecule, and ether solvents having no hydroxyl group in the molecule, amide solvents, and sulfoxide solvents.

[0088] The organic solvent used as the developer in the present invention is preferably an organic solvent having a solubility parameter (SP value) of 7.5 to 11. An organic solvent with a solubility parameter of 7.5 or more increases the development rate of the dissolved portion, while an organic solvent with a solubility parameter of 11 or less can suppress the development rate of the pattern formation portion, and is therefore preferred. The solubility parameter of the organic solvent of the developer is more preferably 8 to 11.

[0089] In the present invention, the solubility parameter (SP value) is calculated by the method proposed by Fedors et al. Specifically, the value is determined by referring to "POLYMER ENGINEERING AND SCIENCE, FEBRUARY, 1974, Vol. 14, No. 2, ROBERT F. FEDORS. (pp. 147-154)." The SP value is a physical property determined by the content of hydrophobic and hydrophilic groups in the molecule, and when a mixed solvent is used, the SP value refers to the value of the mixture.

[0090] Examples of organic solvents that satisfy the above SP values ​​include diethylene glycol monomethyl ether (SP value = 10.7), triethylene glycol monomethyl ether (SP value = 10.7), ethylene glycol monoisopropyl ether (SP value = 10.9), ethylene glycol monobutyl ether (SP value = 10.2), diethylene glycol monobutyl ether (SP value = 10.0), triethylene glycol monobutyl ether (SP value = 10.0), ethylene glycol monoisobutyl ether (SP value = 9.1), ethylene glycol monohexyl ether (SP value = 9.9), diethylene glycol monohexyl ether (SP value = 9.7), diethylene glycol mono-2-ethylhexyl ether (SP value = 9.3), ethylene glycol monoallyl ether (SP value = 10.8), ethylene glycol monophenyl ether (SP value = 10.8), ethylene glycol monobenzyl ether (SP value = 10.9), propylene glycol monomethyl ether (SP value = 10.0), dipropylene glycol monomethyl ether (SP value = 10.0), and dipropylene glycol monomethyl ether (SP value = 10.0). propylene glycol monomethyl ether (SP value = 9.7), tripropylene glycol monomethyl ether (SP value = 9.4), propylene glycol monopropyl ether (SP value = 9.6), dipropylene glycol monopropyl ether (SP value = 9.8), propylene glycol monobutyl ether (SP value = 9.0), dipropylene glycol monobutyl ether (SP value = 9.6), ethylene glycol monomethyl ether acetate (SP value = 10.0), ethylene glycol monoethyl ether acetate ether acetate (SP value = 9.6), ethylene glycol monobutyl ether acetate (SP value = 8.9), diethylene glycol monoethyl ether acetate (SP value = 9.4), diethylene glycol monobutyl ether acetate (SP value = 9.0), propylene glycol monomethyl ether acetate (SP value = 9.4), propylene glycol monoethyl ether acetate (SP value = 9.0), and dipropylene glycol monomethyl ether acetate (SP value = 9.2).

[0091] The organic solvents mentioned above may be used in combination, or may be used in combination with a solvent other than those mentioned above or with water.

[0092] The concentration of the organic solvent (total when a plurality of organic solvents are mixed) in the developer is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more. It is particularly preferred that the developer essentially consists of an organic solvent. The term "essentially consisting of an organic solvent" includes the case where the developer contains trace amounts of a surfactant, an antioxidant, a stabilizer, an antifoaming agent, etc.

[0093] The water content in the developer is preferably 10% by mass or less, more preferably 5% by mass or less, particularly preferably 3% by mass or less, and most preferably substantially no water. By keeping the water content at 10% by mass or less, good development characteristics can be obtained.

[0094] If necessary, an appropriate amount of a surfactant can be added to the developer used in the present invention. The surfactant may be the same as those described above as surfactants used in the photosensitive composition of the present invention. The amount of the surfactant used is usually 0.001 to 5% by mass, preferably 0.005 to 2% by mass, and more preferably 0.01 to 0.5% by mass, based on the total amount of the developer.

[0095] [Development Method] Examples of development methods that can be used include a method in which a substrate is immersed in a tank filled with a developer for a certain period of time (dip method), a method in which a developer is piled up on the surface of a substrate by surface tension and left standing for a certain period of time (puddle method), a method in which a developer is sprayed onto the surface of the substrate (spray method), and a method in which a developer is continuously dispensed onto a substrate rotating at a constant speed while a developer dispenser nozzle is scanned at a constant speed (dynamic dispense method). Furthermore, after the development step, a step of stopping development by replacing the solvent with another solvent may be carried out. The development time is preferably a time required for the cluster compound and the like in the photosensitive layer in the unexposed or exposed areas to be sufficiently dissolved, typically 10 to 300 seconds, more preferably 20 to 120 seconds. The temperature of the developer is preferably 0 to 50°C, more preferably 15 to 35°C. The amount of developer can be appropriately adjusted depending on the development method.

[0096] [Rinsing Step] The present pattern forming method may include, after the developing step, a step of washing with a rinse liquid containing an organic solvent.

[0097] [Rinse Liquid] The organic solvent used in the rinse liquid preferably has a vapor pressure of 0.05 kPa or more and 5 kPa or less, more preferably 0.1 kPa or more and 5 kPa or less, and most preferably 0.12 kPa or more and 3 kPa or less at 20° C. By adjusting the vapor pressure of the organic solvent used in the rinse liquid to 0.05 kPa or more and 5 kPa or less, the temperature uniformity within the wafer surface is improved, and further swelling due to penetration of the rinse liquid is suppressed, thereby improving the dimensional uniformity within the wafer surface.

[0098] Various organic solvents can be used as the rinse solution. However, for the present cluster compound, it is preferable to use a rinse solution containing at least one organic solvent selected from hydrocarbon solvents, ketone solvents, ester solvents, alcohol solvents, amide solvents, and ether solvents, or water. More preferably, after development, a cleaning step is performed using a rinse solution containing at least one organic solvent selected from ketone solvents, ester solvents, alcohol solvents, amide solvents, and hydrocarbon solvents. Even more preferably, after development, a cleaning step is performed using a rinse solution containing at least one organic solvent selected from the group consisting of alcohol solvents and hydrocarbon solvents. Specific examples of ketone solvents, ester solvents, alcohol solvents, amide solvents, ether solvents, and hydrocarbon solvents used as the rinse solution are the same as those described above for the developer. It is particularly preferable to use a rinse solution containing at least one organic solvent selected from the group consisting of monohydric alcohol solvents, hydrocarbon solvents, and amide solvents.

[0099] Here, examples of the monohydric alcohol solvent used in the rinsing step after development include linear, branched, and cyclic monohydric alcohols. Specific examples include 1-butanol, 2-butanol, 3-methyl-1-butanol, tert-butyl alcohol, isopropyl alcohol, cyclopentanol, and cyclohexanol, with 1-butanol, 2-butanol, 3-methyl-1-butanol, and isopropyl alcohol being preferred. Examples of the hydrocarbon solvent include aromatic hydrocarbon solvents such as toluene and xylene, and aliphatic hydrocarbon solvents such as octane, decane, and dodecane. Examples of the amide solvent include N,N-dimethylformamide.

[0100] The above-mentioned components may be mixed in plural, or may be mixed with an organic solvent other than those mentioned above.

[0101] The organic solvent may be mixed with water, but the water content in the rinse solution is usually 30% by mass or less, preferably 10% by mass or less, more preferably 5% by mass or less, and particularly preferably 3% by mass or less. Most preferably, the rinse solution does not contain water. By keeping the water content at 30% by mass or less, good development properties can be obtained.

[0102] The rinse solution may contain an appropriate amount of a surfactant, which may be the same as those used in the photosensitive composition described above, and the amount of surfactant used is usually 0.001 to 5 mass %, preferably 0.005 to 2 mass %, and more preferably 0.01 to 0.5 mass %, based on the total amount of the rinse solution.

[0103] [Rinsing Method] In the rinsing step, the developed pattern-formed substrate is washed with a rinse solution containing the organic solvent. The washing method is not particularly limited, but examples include a method in which the rinse solution is continuously applied to a substrate rotating at a constant speed (spin coating method), a method in which the substrate is immersed in a tank filled with the rinse solution for a certain period of time (dipping method), and a method in which the rinse solution is sprayed onto the substrate surface (spray method). Among these, the spin coating method is preferred for washing, and after washing, the substrate is rotated at a speed of 2000 to 4000 rpm to remove the rinse solution from the substrate. The substrate rotation time can be set depending on the rotation speed within a range that achieves complete removal of the rinse solution from the substrate, but is typically 10 seconds to 3 minutes. Rinsing is preferably performed at room temperature. The rinse time is preferably set so that no developing solvent remains on the substrate, typically 10 to 300 seconds, more preferably 20 to 120 seconds. The temperature of the rinse solution is preferably 0 to 50°C, and even more preferably 15 to 35°C. The amount of the rinse solution can be adjusted appropriately depending on the rinse method.

[0104] [Post-treatment step] After the development treatment or rinsing treatment, a treatment can be performed using a supercritical fluid to remove the developer or rinsing solution adhering to the pattern. Furthermore, after the development treatment, rinsing treatment, or treatment with a supercritical fluid, a heat treatment can be performed to remove the solvent remaining in the pattern. The heating temperature and time are not particularly limited as long as a good resist pattern can be obtained, and are usually 40 to 160°C and 10 seconds to 3 minutes. The heat treatment may be performed multiple times.

[0105] [Uses] The present photosensitive composition and the present pattern formation method are suitable for use in the production of semiconductor microcircuits, such as the manufacture of VLSIs and high-capacity microchips. During the production of semiconductor microcircuits, the resist film on which the pattern has been formed is subjected to circuit formation and etching, and the remaining resist film portion is ultimately removed with a solvent or the like. Therefore, unlike so-called permanent resists used in printed circuit boards and the like, no resist film derived from the present photosensitive composition remains in the final product, such as a microchip.

[0106] An example of the present invention will be described below. However, the present invention is not limited to this example. In the example, "parts" and "%" are by mass unless otherwise specified.

[0107] The following compounds 1 to 3 were prepared to obtain Examples 1 to 3. The composition and ligand structure of each compound are as follows: 1 Measurement was performed by H-NMR (400 MHz). Peak splitting is represented by the following abbreviations: brs stands for broad singlet, brm for broad multiplet, m for multiplet, s for singlet, d for doublet, t for triplet, and q for quartet.

[0108] <Compound 1> Under a nitrogen atmosphere, 24.83 g of 2-ethylhexyl chloroformate (130 mmol, manufactured by Tokyo Chemical Industry Co., Ltd.) and 400 ml of dichloromethane (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were placed in a reaction vessel, and 2.89 g of N,N-diisopropylethylamine (13 mmol, manufactured by Tokyo Chemical Industry Co., Ltd.) and a dichloromethane solution (80 ml) of 25.2 g of 4-amino-2,6-dichlorophenol (0.14 mmol, manufactured by Tokyo Chemical Industry Co., Ltd.) were added dropwise at 0°C. The mixture was stirred at room temperature for 2 hours. Thereafter, 0.5 ml of water was added, and the mixture was stirred for 10 minutes. After concentration under reduced pressure, the residue was purified by silica gel column chromatography to obtain a yellow-white powder (27.93 g). NMR analysis of the obtained yellow-white powder revealed that it had the structure represented by formula 3 below.

[0109] H-NMR (CDCl 3 ) 7.36 (brs, 2H), 6.57 (brs, 1H), 5.73 (s, 1H), 4.16-4.01 (m, 2H), 1.65-1.52 (m, 1H), 1.46-1.20 (m, 8H), 0.99-0.82 (m, 6H).

[0110]

[0111] To a reaction vessel, 7.92 g (20 mmol) of the compound represented by Formula 3 above, 3.39 g (10 mmol) of triphenylbismuth (manufactured by Tokyo Chemical Industry Co., Ltd.), and 265 ml of dehydrated toluene (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added, and the mixture was heated and stirred at 140°C for 57 hours under a nitrogen atmosphere. The resulting reaction solution was concentrated under reduced pressure, and the residue was reprecipitated with THF-hexane to obtain a yellow-brown powder (4.33 g). H-NMR analysis and elemental analysis (Bi 34%) of the resulting yellow-brown powder revealed that the ratio of Bi to the compound represented by Formula 3 above was Bi:compound represented by Formula 3 = 1:1.2. It was estimated that oxygen atoms bridged the bismuth to form a cluster structure (Compound 1), as shown in Formula 4 below.

[0112] H-NMR (CDCl 3 ) 8.25-5.23 (brm, 3H), 4.49-3.49 (brs, 2H), 1.83-1.50 (brs, 1H), 1.50-1.07 (brm, 8H), 1.07-0.25 (brm, 6H).

[0113] (The above formula 4 is a mixture containing different cluster structures where n is 2 or more and 6 or less.)

[0114] <Compound 2> Under a nitrogen atmosphere, 24.83 g of normal octyl chloroformate (130 mmol, manufactured by Tokyo Chemical Industry Co., Ltd.) and 400 ml of dichloromethane (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were placed in a reaction vessel, and 2.89 g of N,N-diisopropylethylamine (13 mmol, manufactured by Tokyo Chemical Industry Co., Ltd.) was added dropwise at 0°C, followed by a dichloromethane solution (80 ml) of 25.2 g of 4-amino-2,6-dichlorophenol (0.14 mmol, manufactured by Tokyo Chemical Industry Co., Ltd.), and the mixture was stirred at room temperature for 2 hours. Thereafter, 0.5 ml of water was added, and the mixture was stirred for 10 minutes. After concentration under reduced pressure, the residue was purified by silica gel column chromatography to obtain a white powder (27.93 g). NMR analysis of the obtained white powder revealed that it had the structure represented by the following formula 5.

[0115] H-NMR (CDCl 3) 7.36 (s, 2H), 6.43 (brs, 1H), 5.63 (s, 1H), 4.15 (t, J = 6.8Hz, 2H), 1.66 (tt, J = 6.9Hz, 2H), 1.45-1.14 (m, 10H), 0.89 (t, J = 6.8Hz, 3H).

[0116]

[0117] To a reaction vessel, 7.18 g (20 mmol) of the compound described in Formula 5 above, 3.03 g (10 mmol) of triphenylbismuth (manufactured by Tokyo Chemical Industry Co., Ltd.), and 236 ml of dehydrated toluene (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added, and the mixture was heated and stirred at 140°C for 48 hours under a nitrogen atmosphere. The resulting reaction solution was concentrated under reduced pressure, and the residue was reprecipitated with THF-hexane to obtain a black powder (2.83 g). H-NMR analysis and elemental analysis (Bi 40%) of the obtained black powder revealed that the ratio of Bi to the compound described in Formula 5 above was Bi:compound of Formula 5 = 1:0.9. It was estimated that oxygen atoms bridged the bismuth to form a cluster structure (Compound 2), as described in Formula 6 below.

[0118] H-NMR (CDCl 3 ) 8.33-5.02 (brm, 3H), 4.55-3.79 (brs, 2H), 2.09-1.51 (brm, 2H), 1.51-1.00 (brm, 10H), 1.00-0.23 (brm, 3H).

[0119] (The above formula 6 is a mixture containing different cluster structures where n is 2 or more and 6 or less.)

[0120] <Compound 3> Under a nitrogen atmosphere, 25.52 g of normal propyl chloroformate (140 mmol, manufactured by Tokyo Chemical Industry Co., Ltd.) and 500 ml of dichloromethane (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were placed in a reaction vessel, and 27 ml of N,N-diisopropylethylamine (140 mmol, manufactured by Tokyo Chemical Industry Co., Ltd.) was added dropwise at 0°C, followed by a dichloromethane solution (80 ml) of 24.83 g of 4-amino-2,6-dichlorophenol (0.14 mmol, manufactured by Tokyo Chemical Industry Co., Ltd.), and the mixture was stirred at room temperature for 2 hours. Thereafter, 0.5 ml of water was added, and the mixture was stirred for 10 minutes. After concentration under reduced pressure, the residue was purified by silica gel column chromatography to obtain a white powder (16.52 g). NMR analysis of the obtained white powder revealed that it had the structure represented by formula 7 below.

[0121] H-NMR (CDCl 3 ) 7.36 (s, 2H), 6.46 (brs, 1H), 5.64 (s, 1H), 4.12 (t, J = 6.9Hz, 2H), 1.69 (tq, J = 6.9Hz, 2H), 0.97 (t, J = 7.0Hz, 3H).

[0122]

[0123] To a reaction vessel were added 8.13 g (30 mmol) of the compound represented by Formula 7 above, 4.37 g (10 mmol) of triphenylbismuth (manufactured by Tokyo Chemical Industry Co., Ltd.), and 265 ml of dehydrated toluene (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), and the mixture was heated and stirred at 140°C for 48 hours under a nitrogen atmosphere. The resulting reaction solution was concentrated under reduced pressure, and the residue was reprecipitated with THF-hexane to obtain a whitish-green powder (4.47 g). H-NMR analysis and elemental analysis (Bi 47%) of the resulting whitish-green powder revealed that the ratio of Bi to the compound represented by Formula 7 above was Bi:compound represented by Formula 7 = 1:0.84. It was estimated that oxygen atoms bridged the bismuth to form a cluster structure (compound 3), as shown in Formula 8 below.

[0124] H-NMR(THF-d 8 ) 8.97-7.78 (brm, 1H), 7.73-6.25 (brm, 2H), 4.02 (brs, 2H), 1.68-1.36 (brm, 2H. THF-d 8The integral value is estimated because it overlaps with the impurity peak of 1.13-0.63 (brm, 3H). 3 It was poorly soluble in

[0125] (The above formula 8 is a mixture containing different cluster structures where n is 2 or more and 6 or less.)

[0126] <Preparation of Photosensitive Composition (Resist Solution)> Each of the above compounds 1 to 3 was dissolved in ethyl lactate to a concentration of 3% by mass, and the solution was filtered through a 0.2 μm filter to obtain a resist solution.

[0127] The prepared resist solution was applied to a pattern formation substrate (silicon wafer) by spin coating to form a resist film with a thickness of approximately 50 nm. The resulting resist film was baked at 90°C for 90 seconds, and then patterned using an electron beam lithography system (electron beam acceleration voltage: 100 keV).

[0128] <Development> After pattern writing, Compounds 1 to 3 were developed with ethyl lactate (25° C., 60 seconds) to obtain negative patterns, which were designated as Examples 1 to 3, respectively.

[0129] <Measurement of Sensitivity> Electron beam (EB) exposure was performed at different doses, and the film thickness of the developed pattern was measured with a contact step gauge. The dose of electron beam at which the increase in film thickness was maximized was determined as the sensitivity. The results are shown in Table 1 below.

[0130] Comparative Example 1 Polystyrene (PS, weight average molecular weight 4000) manufactured by Aldrich was dissolved in propylene glycol monomethyl ether acetate to a concentration of 2% by mass, and the solution was filtered through a 0.2 μm filter to prepare a resist solution.

[0131] The resist solution of Comparative Example 1 was evaluated in the same manner as in Examples 1 to 3, and the results are shown in Table 1 below.

[0132]

[0133] From the results in Table 1, it was confirmed that Examples 1 to 3 had higher sensitivity than Comparative Example 1, and that Examples 1 to 3 had lower exposure amounts than Comparative Example 1.

[0134] <Resolution Evaluation> Resolution evaluation was performed on Examples 1 to 3 and Comparative Example 1 using an electron beam lithography device. Resolution was evaluated by drawing line and space (line:space=1:1) patterns with hp (half pitch) of 100 nm and 50 nm, developing the patterns, and observing each pattern with a scanning electron microscope. The results are shown in Table 2 below. Cases where a line and space pattern with hp of 100 nm or 50 nm could be confirmed were evaluated as "A," and cases where no pattern could be confirmed were evaluated as "B."

[0135]

[0136] From the above results, it was found that the photosensitive composition of the present invention can form a fine pattern of hp 50 nm and exhibits extremely high sensitivity to electron beam (EB) irradiation. In contrast, in Comparative Example 1, a fine pattern of hp 100 nm could be formed, but a fine pattern of hp 50 nm could not be formed.

Claims

1. A photosensitive composition comprising a metal cluster compound, which is a compound forming a cluster centered on a metal element, and which is composed of a metal element and a ligand represented by the following general formula (1), and which optionally contains oxygen and / or a hydroxyl group. (In the above formula (1), X 1 and X 2 are each independently a halogen atom and may be the same or different; R 1 , R 2 , R 3 are each independently hydrogen or any substituent, and may be the same or different.

2. The photosensitive composition according to claim 1, wherein the ligand is a ligand represented by the following general formula (2): (In the above formula (2), X 1 and X 2 are each independently a halogen atom and may be the same or different; R 1 , R 3 , R 4 are each independently hydrogen or any substituent, and may be the same or different.

3. The photosensitive composition according to claim 1, wherein the number of metal elements in the metal cluster compound is 2 to 12.

4. The photosensitive composition according to claim 1, wherein the metal cluster compound is in an electrically neutral state.

5. The photosensitive composition according to claim 1 or 2, wherein the metal element is bismuth.

6. X in the formula (1) or (2) 1 and X 2 3. The photosensitive composition according to claim 1, wherein both are chlorine.

7. R in the formula (1) or (2) 1 , R 3 3. The photosensitive composition of claim 1, wherein both are hydrogen.

8. R in the above formula (2) 4 3. The photosensitive composition according to claim 2, wherein the hydrocarbon group has 1 to 20 carbon atoms.

9. R in the above formula (2) 4 3. The photosensitive composition of claim 2, wherein is a linear or branched saturated hydrocarbon group.

10. The photosensitive composition according to claim 1 or 2, further comprising a photoacid generator which generates an acid under the action of actinic radiation.

11. The photosensitive composition according to claim 1 or 2, wherein the molecular weight of the metal cluster compound is from 300 to 8,000.

12. The photosensitive composition according to claim 1 or 2, further comprising an organic solvent.

13. The photosensitive composition according to claim 1 or 2, wherein the content of the metal cluster compound is 1 to 30% by mass.

14. The photosensitive composition according to claim 11, wherein the actinic radiation has a wavelength of 6.5 to 13.5 nm.

15. A pattern forming method comprising a step of forming a photosensitive layer on a substrate by spin coating using the photosensitive composition according to claim 1 or 2.

16. A pattern formation method comprising the steps of: forming a photosensitive layer on a substrate using the photosensitive composition according to claim 1 or 2; irradiating predetermined regions of the photosensitive layer with actinic radiation to perform pattern exposure; and developing the exposed photosensitive layer with a developer to selectively remove exposed or unexposed portions of the photosensitive layer.

17. The pattern formation method according to claim 15, wherein the developer is an organic solvent having a solubility parameter (SP value) of 7.5 to 11.

18. A metal cluster compound which is a compound forming a cluster centered around a metal element and which is composed of a metal element and a ligand represented by the following general formula (2): (In the above formula (2), X 1 and X 2 are each independently a halogen atom and may be the same or different; R 1 , R 3 , R 4 are each independently hydrogen or any substituent, and may be the same or different.

19. The metal cluster compound according to claim 18, wherein the number of metal elements in the metal cluster compound is 2 to 12.

20. The metal cluster compound according to claim 18 or 19, wherein the metal element is bismuth.

21. X in the above formula (2) 1 and X 2 The metal cluster compound according to claim 18 or 19, wherein both are chlorine.

22. R in the above formula (2) 1 , R 3 The metal cluster compound according to claim 18 or 19, wherein both are hydrogen.

23. R in the above formula (2) 4 20. The metal cluster compound according to claim 18, wherein the carbon number of the hydrocarbon group is from 1 to 20.

24. R in the above formula (2) 4 20. The metal cluster compound according to claim 18 or 19, characterized in that is a linear or branched saturated hydrocarbon group.

Citation Information

Patent Citations

  • Negative resist composition, resist pattern forming method, and complex

    JP2015108781A

  • Organically modified metal oxide nanoparticle, solution containing organically modified metal oxide nanoparticle, resist composition containing organically modified metal oxide nanoparticle and resist pattern formation method

    JP2021102604A

  • Ionic salt, and radiation-sensitive resist composition

    JP2023013561A

  • Organic tin compound, method for producing same, liquid composition for forming EUV resist film using same, and method for forming EUV resist film

    WO2022102636A1

Cited By

  • Compound, photosensitive composition containing said compound, pattern forming method using said composition, substrate, and method for producing substrate

    WO2026009885A1