Coating liquid and method for producing adhesive layer for secondary battery

The coating liquid with a specific elastic modulus distribution and core-shell structured adhesive particles addresses nozzle clogging in inkjet-based adhesive layer formation for secondary batteries, achieving high adhesive strength and intermittent performance.

WO2024202962A1PCT designated stage expired Publication Date: 2024-10-03ZEON CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/007974
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-04
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

The inkjet method for forming adhesive layers in secondary batteries often experiences nozzle clogging due to intermittent ejection, particularly when using high adhesive strength materials, which reduces performance.

Method used

A coating liquid with a specific elastic modulus distribution in the dry product, surface tension within a certain range, and adhesive particles with a core-shell structure and glass transition temperature below 25°C, applied using an inkjet method to achieve high intermittent discharge performance and adhesive strength.

Benefits of technology

The coating liquid enables efficient and reliable formation of adhesive layers with high adhesive strength and improved intermittent ejection performance, reducing nozzle clogging and enhancing the adhesion between battery components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

Provided is a coating liquid for a secondary battery, wherein in a cross-section of a dried product of the coating liquid, elastic modulus as determined by measurement via atomic force microscopy at room temperature is not less than 5% but less than 50% in the region of not less than 5 MPa. The coating liquid preferably exhibits a surface tension of 30-50 mN / m at 30°C. Preferably, the coating liquid includes adhesion particles, and includes adhesion particles having a core-shell structure as some or all of the adhesion particles. Also provided is a method for producing an adhesive layer for a secondary battery, said method comprising applying the coating liquid via an inkjet method.
Need to check novelty before this filing date? Find Prior Art

Description

Coating liquid and method for manufacturing adhesive layer for secondary battery

[0001] The present invention relates to a coating liquid suitable for producing an adhesive layer for a secondary battery, and a method for producing an adhesive layer for a secondary battery.

[0002] Secondary batteries, such as nonaqueous secondary batteries such as lithium-ion secondary batteries, generally include battery components such as a positive electrode, a negative electrode, and a separator that separates the positive electrode and the negative electrode to prevent short-circuiting between them. These battery components are often formed as layered structures. They are required to be held in close proximity to each other within the secondary battery. Therefore, an adhesive layer may be provided between these battery components to bond them together. Recently, one method for efficiently forming such an adhesive layer has been investigated: inkjet printing, in which a coating liquid for forming the adhesive layer is ejected from a nozzle as fine droplets (see, for example, Patent Documents 1 and 2). When forming an adhesive layer using the inkjet method, a coating liquid that is an adhesive layer material is ejected from the nozzle of a coating machine.

[0003] International Publication No. WO 2022 / 209997 (corresponding publication: European Patent Application Publication No. 4318633) International Publication No. WO 2020 / 045246 (corresponding publication: U.S. Patent Application Publication No. 2021 / 296732)

[0004] When forming an adhesive layer by an inkjet method, nozzle clogging becomes a problem. In particular, when forming an adhesive layer, due to process reasons, it is frequently necessary to perform intermittent ejection, in which ejection is stopped for a long period of time and then restarted. When ejection is restarted after such a stop, nozzle clogging becomes a problem. Such a decrease in intermittent ejection performance is particularly noticeable when an adhesive layer material with high adhesive strength is used as the coating liquid.

[0005] Therefore, an object of the present invention is to provide a coating liquid suitable for producing an adhesive layer for a secondary battery, which can achieve both high intermittent discharge performance and high adhesive strength, and a method for producing an adhesive layer for a secondary battery that can be easily carried out intermittently and can achieve high adhesive strength.

[0006] The present inventors have conducted research to solve the above-mentioned problems, and have found that a coating liquid for forming an adhesive layer that exhibits a specific distribution of elastic modulus in a cross section of the dried product after drying can solve the above-mentioned problems, and have completed the present invention.

[0007] (1) A coating liquid for a secondary battery, wherein a region in a cross section of a dried product of the coating liquid where the modulus of elasticity is 5 MPa or more as measured by atomic force microscope observation at room temperature is 5% or more and less than 50%. (2) The coating liquid according to (1), wherein the surface tension at 30°C is 30 mN / m or more and 50 mN / m or less. (3) The coating liquid according to (1) or (2), wherein the coating liquid contains adhesive particles, and wherein some or all of the adhesive particles have a core-shell structure. (4) The coating liquid according to (3), wherein the adhesive particles other than the core-shell structure contain particles having a glass transition temperature Tg of less than 25°C. (5) The coating liquid according to (1) or (2), wherein the coating liquid contains adhesive particles, and wherein the adhesive particles include particles having a glass transition temperature Tg of less than 25°C. (6) The coating liquid according to any one of (1) to (5), wherein the coating liquid contains adhesive particles, and wherein the particle diameter of the adhesive particles is 100 nm or more and 1000 nm or less. (7) A method for producing an adhesive layer for a secondary battery, the method comprising applying the coating liquid according to any one of (1) to (6) by an inkjet method.

[0008] According to the present invention, there are provided a coating liquid suitable for producing an adhesive layer for a secondary battery, which can achieve both high intermittent discharge performance and high adhesive strength, and a method for producing an adhesive layer for a secondary battery, which can be easily carried out intermittently and can achieve high adhesive strength.

[0009] The present invention will be described in detail below with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and can be implemented with any modifications within the scope of the claims of the present invention and their equivalents.

[0010] (Coating Liquid: Elastic Modulus) The coating liquid of the present invention is a coating liquid for a secondary battery, and in a cross section of a dried product thereof, the region where the elastic modulus is 5 MPa or more as measured by atomic force microscope (AFM) observation at room temperature falls within a specific range.

[0011] The dried material used for measuring the elastic modulus can be obtained by storing approximately 1.5 g of coating liquid in a dish-shaped container and drying it at 25°C for 24 hours or more. The cross-section of the dried material can be obtained by cutting the dried material using a microtome so that the cross-section is in the thickness direction of the dried material, resulting in slices approximately 1 μm thick. Measurement of the elastic modulus by AFM can be performed using an atomic force microscope (e.g., manufactured by Bruker, product name "Dimension Icon") equipped with a cantilever such as a silicon cantilever. The measurement field is 5 μm x 5 μm, and measurements can be performed at approximately 16,000 to 17,000 measurement points. The number of measurement points with a value of 5 MPa or higher is determined, and the percentage of this number relative to the total number of measurement points can be used to determine the proportion of the region with a value of 5 MPa or higher. The percentage of the remaining number can be used to determine the proportion of the region with a value of less than 5 MPa.

[0012] The inventors have discovered that when the dried product of the coating liquid for forming the adhesive layer shows such a distribution of elastic modulus in cross section, the resulting dried product can exhibit good adhesive strength and have high intermittent discharge performance.

[0013] From the viewpoint of achieving the above-mentioned effects, the lower limit of the proportion of the region having an elastic modulus of 5 MPa or more is preferably 10% or more, more preferably 20% or more. The lower limit of the proportion of the region having an elastic modulus of less than 5 MPa is 50% or more, preferably 55% or more, more preferably 80% or more, and the upper limit is 95% or less.

[0014] A coating liquid having such a specific dry matter elastic modulus distribution can be easily obtained by using a component containing adhesive particles and adjusting the type and amount of the adhesive particles. In particular, a desired dry matter elastic modulus distribution can be obtained by combining a particulate polymer having a core-shell structure with a particulate polymer not having a core-shell structure as adhesive particles and adjusting the ratio between them. In addition, the dry matter elastic modulus distribution can also be adjusted by changing the ratio of an anti-drying agent contained in the coating liquid.

[0015] (Coating Liquid: Other Physical Properties) The coating liquid of the present invention preferably has a surface tension at 30°C of 30 mN / m or more, more preferably 35 mN / m or more, and preferably 50 mN / m or less, more preferably 45 mN / m or less. Having a surface tension in this range makes the coating liquid suitable for coating by the inkjet method. The surface tension can be measured by the platinum plate method using a surface tensiometer (for example, the high-performance surface tensiometer "DY-500" manufactured by Kyowa Interface Science Co., Ltd.).

[0016] (Materials Constituting the Coating Fluid) In a preferred example, the coating fluid of the present invention can be a dispersion containing adhesive particles that function as an adhesive and a dispersion medium.

[0017] (Adhesive Particles) The coating liquid of the present invention may contain particles having a glass transition temperature Tg of less than 25°C as some or all of the adhesive particles. More preferably, some of the adhesive particles contain particles having a glass transition temperature of less than 25°C. By adjusting the proportion of particles having such a low glass transition temperature among all the adhesive particles, a desired dry product elastic modulus distribution can be obtained and the adhesive strength of the adhesive layer can also be adjusted. The glass transition temperature can be determined from a differential scanning calorimetry (DSC) curve obtained by measuring the temperature range of -100°C to 200°C at a heating rate of 10°C / min under conditions specified in JIS Z8703 using a differential thermal analyzer (for example, an "EXSTAR DSC6220" manufactured by SII NanoTechnology Inc.).

[0018] The particle diameter of the adhesive particles contained in the coating liquid of the present invention is preferably 100 nm or more, more preferably 200 nm or more, and preferably 1000 nm or less, more preferably 800 nm or less. A particle diameter within this range facilitates high intermittent discharge performance in inkjet coating and high adhesive strength with the resulting adhesive layer. The particle diameter referred to here is the volume-average particle diameter. The particle diameter can be measured by laser diffraction. Specifically, the volume-average particle diameter D50 (nm) can be determined as the particle diameter at which the cumulative volume calculated from the smallest diameter side is 50% in the particle size distribution (volume basis) obtained using a laser diffraction particle size distribution analyzer (e.g., Beckman Coulter, Inc., product name "LS-13 320"). When the coating liquid of the present invention contains adhesive particles of multiple types with different particle diameters, the volume-average particle diameter of the entire multiple types of adhesive particles is preferably within this range.

[0019] The coating liquid may contain adhesive particles having a core-shell structure as some or all of the adhesive particles. The adhesive particles may be a particulate polymer, i.e., a polymer having a particulate shape. More specifically, the adhesive particles may include particles having a core-shell structure and particles not having a core-shell structure, and the particles not having a core-shell structure may include particles whose glass transition temperature Tg is lower than 25°C.

[0020] (Adhesive particles: particulate polymer having a core-shell structure) The particulate polymer having a core-shell structure as the adhesive particles has a core part and a shell part covering the outer surface of the core part. By using the particulate polymer having a core-shell structure, the adhesiveness of the obtained adhesive layer can be further improved.

[0021] Here, the shell portion may cover the entire outer surface of the core portion or may cover only a portion of the outer surface of the core portion. Even if the outer surface of the core portion appears to be completely covered by the shell portion, the shell portion is considered to be a shell portion that partially covers the outer surface of the core portion as long as it has holes that communicate between the inside and outside of the shell portion.

[0022] The particulate polymer may have any constituent element other than the core and shell portions described above, as long as the intended effect is not significantly impaired. Specifically, for example, the particulate polymer may have a portion formed of a polymer different from the core portion inside the core portion. As a specific example, seed particles used when producing the particulate polymer by seed polymerization may remain inside the core portion. However, from the viewpoint of significantly exhibiting the intended effect, it is preferable that the particulate polymer has only the core portion and the shell portion.

[0023] (Core Portion) The glass transition temperature of the polymer of the core portion of the particulate polymer is preferably −50° C. or higher, more preferably −45° C. or higher, even more preferably −40° C. or higher, and preferably lower than 80° C., more preferably 10° C. or lower, and even more preferably 0° C. or lower. When the glass transition temperature of the polymer of the core portion is equal to or higher than the above lower limit, the inkjet ejection characteristics can be improved. On the other hand, when the glass transition temperature of the polymer of the core portion is equal to or lower than the above upper limit, the adhesiveness of the obtained adhesive layer can be further improved. The glass transition temperature of the polymer of the core portion can be adjusted, for example, by changing the type and ratio of the monomers used in preparing the polymer of the core portion.

[0024] Examples of monomers used to prepare the core polymer include vinyl chloride monomers such as vinyl chloride and vinylidene chloride; vinyl acetate monomers such as vinyl acetate; aromatic vinyl monomers such as styrene, α-methylstyrene, styrene sulfonic acid, butoxystyrene, and vinylnaphthalene; vinylamine monomers such as vinylamine; vinylamide monomers such as N-vinylformamide and N-vinylacetamide; methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, and methyl methacrylate. Examples of suitable (meth)acrylic acid ester monomers include fluorine-free (meth)acrylic acid ester monomers such as ethyl methacrylate, butyl methacrylate, and cyclohexyl methacrylate; (meth)acrylamide monomers such as acrylamide and methacrylamide; (meth)acrylonitrile monomers such as acrylonitrile and methacrylonitrile; fluorine-containing (meth)acrylic acid ester monomers such as 2-(perfluorohexyl)ethyl methacrylate and 2-(perfluorobutyl)ethyl acrylate; maleimide; and maleimide derivatives such as phenylmaleimide. These may be used alone or in combination of two or more in any ratio. In the present invention, (meth)acrylic refers to acrylic and / or methacrylic, and (meth)acrylonitrile refers to acrylonitrile and / or methacrylonitrile.

[0025] Among these monomers, it is preferable to use at least a (meth)acrylic acid ester monomer as the monomer used to prepare the core polymer, from the viewpoint of further increasing the adhesive strength achieved by the adhesive layer, and a combination of a (meth)acrylic acid ester monomer and an aromatic vinyl monomer, or a combination of a (meth)acrylic acid ester monomer and a (meth)acrylonitrile monomer is more preferable, and a combination of a (meth)acrylic acid ester monomer and an aromatic vinyl monomer is particularly preferable. That is, the core polymer preferably contains at least a (meth)acrylic acid ester monomer unit, more preferably a (meth)acrylic acid ester monomer unit and an aromatic vinyl monomer unit or a (meth)acrylonitrile monomer unit, and even more preferably a (meth)acrylic acid ester monomer unit and an aromatic vinyl monomer unit. In the present invention, "containing a monomer unit" means that "a polymer obtained using that monomer contains a repeating unit derived from the monomer." In the present invention, the term "(meth)acrylic acid ester monomer" refers to a monofunctional (meth)acrylic acid ester monomer having only one polymerization reactive group.

[0026] From the viewpoint of further increasing the adhesive strength achieved by the adhesive layer, the proportion of (meth)acrylic acid ester monomer units in the core polymer is preferably 5% by mass or more, more preferably 10% by mass or more, particularly preferably 20% by mass or more, and preferably 80% by mass or less, and more preferably 70% by mass or less, based on 100% by mass of all repeating units (total monomer units) contained in the core polymer. Furthermore, when the core polymer contains (meth)acrylic acid ester monomer units and aromatic vinyl monomer units, from the viewpoint of further increasing the adhesive strength achieved by the adhesive layer, the proportion of aromatic vinyl monomer units in the core polymer is preferably 15% by mass or more, more preferably 20% by mass or more, particularly preferably 25% by mass or more, and preferably 95% by mass or less, more preferably 80% by mass or less, and particularly preferably 70% by mass or less, based on 100% by mass of all repeating units (total monomer units) contained in the core polymer.

[0027] The core polymer may also contain an acid group-containing monomer unit. Examples of the acid group-containing monomer include a monomer having an acid group, such as a monomer having a carboxylic acid group, a monomer having a sulfonic acid group, or a monomer having a phosphoric acid group.

[0028] Examples of monomers having a carboxylic acid group include monocarboxylic acids and dicarboxylic acids. Examples of monocarboxylic acids include acrylic acid, methacrylic acid, and crotonic acid. Examples of dicarboxylic acids include maleic acid, fumaric acid, and itaconic acid. Examples of monomers having a sulfonic acid group include vinyl sulfonic acid, methyl vinyl sulfonic acid, (meth)allyl sulfonic acid, (meth)acrylic acid-2-ethyl sulfonate, 2-acrylamido-2-methylpropanesulfonic acid, and 3-allyloxy-2-hydroxypropanesulfonic acid. Examples of monomers having a phosphate group include 2-(meth)acryloyloxyethyl phosphate, methyl-2-(meth)acryloyloxyethyl phosphate, and ethyl-2-(meth)acryloyloxyethyl phosphate. In the present invention, (meth)allyl means allyl and / or methallyl, and (meth)acryloyl means acryloyl and / or methacryloyl. Among these, as the acid group-containing monomer, a monomer having a carboxylic acid group is preferred, among which a monocarboxylic acid is preferred, and (meth)acrylic acid is more preferred. Furthermore, the acid group-containing monomer may be used alone or in combination of two or more kinds in any ratio.

[0029] Furthermore, the proportion of the acid group-containing units in the core polymer is preferably 0.1% by mass or more, more preferably 1% by mass or more, and preferably 15% by mass or less, and more preferably 10% by mass or less, based on 100% by mass of all repeating units (total monomer units) contained in the core polymer. By keeping the proportion of the acid group-containing units within the above range, the dispersibility of the core polymer can be improved during preparation of the particulate polymer, and it can be made easier to form a shell portion that partially covers the outer surface of the core polymer.

[0030] In addition to the above-mentioned monomer units, the core polymer preferably contains crosslinkable monomer units. The crosslinkable monomer is a monomer that can form a crosslinked structure during or after polymerization by heating or irradiation with energy rays.

[0031] Examples of crosslinkable monomers include polyfunctional monomers having two or more polymerization reactive groups. Examples of such polyfunctional monomers include divinyl monomers such as divinylbenzene, 1,3-butadiene, isoprene, and allyl methacrylate; di(meth)acrylic acid ester monomers such as ethylene dimethacrylate, diethylene glycol dimethacrylate, ethylene glycol dimethacrylate, diethylene glycol diacrylate, and 1,3-butylene glycol diacrylate; tri(meth)acrylic acid ester monomers such as trimethylolpropane trimethacrylate and trimethylolpropane triacrylate; ethylenically unsaturated monomers containing epoxy groups such as allyl glycidyl ether and glycidyl methacrylate; and γ-methacryloxypropyltrimethoxysilane. Among these, di(meth)acrylic acid ester monomers are more preferred. These may be used alone or in combination of two or more in any ratio.

[0032] Furthermore, the proportion of the crosslinkable monomer units in the core polymer is preferably 0.1% by mass or more, preferably 10% by mass or less, more preferably 5% by mass or less, and particularly preferably 3% by mass or less, based on 100% by mass of all repeating units (total monomer units) contained in the core polymer. By keeping the proportion of the crosslinkable monomer units within the above range, the adhesive strength achieved by the adhesive layer can be further increased.

[0033] (Shell Portion) The glass transition temperature of the polymer of the shell portion of the particulate polymer is preferably 50°C or higher, more preferably 53°C or higher, and preferably 200°C or lower, more preferably 120°C or lower, and even more preferably 105°C or lower. If the glass transition temperature of the polymer of the shell portion is equal to or higher than the above lower limit, the inkjet ejection characteristics can be further improved. On the other hand, if the glass transition temperature of the polymer of the shell portion is equal to or lower than the above upper limit, the particulate polymer becomes appropriately soft, and the adhesive strength achieved by the adhesive layer can be further increased. The glass transition temperature of the polymer of the shell portion can be adjusted, for example, by changing the type and ratio of the monomers used to prepare the polymer of the shell portion.

[0034] From the viewpoint of maintaining the shape of the particulate polymer in the resulting secondary battery and suppressing an increase in resistance, the glass transition temperature of the polymer in the shell portion is preferably at least 25°C higher, and more preferably at least 50°C higher, than the glass transition temperature of the polymer in the core portion described above.

[0035] Examples of the monomers used to prepare the polymer for the shell portion include the same monomers as those exemplified as the monomers that can be used to produce the polymer for the core portion. Furthermore, such monomers may be used alone or in combination of two or more types in any ratio.

[0036] Among these monomers, from the viewpoint of further increasing the adhesive strength achieved by the adhesive layer, it is preferable to use at least one of a (meth)acrylic acid ester monomer and an aromatic vinyl monomer as the monomer used to prepare the polymer for the shell portion, and it is more preferable to use both a (meth)acrylic acid ester monomer and an aromatic vinyl monomer. That is, it is preferable that the polymer for the shell portion contains at least one of a (meth)acrylic acid ester monomer unit and an aromatic vinyl monomer unit, and it is more preferable that it contains both a (meth)acrylic acid ester monomer unit and an aromatic vinyl monomer unit.

[0037] From the viewpoint of further increasing the adhesive strength achieved by the adhesive layer, the proportion of (meth)acrylic acid ester monomer units in the polymer of the shell portion is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 32.5% by mass or more, with all repeating units (all monomer units) contained in the polymer of the shell portion being 100% by mass, and is preferably 90% by mass or less, and more preferably 85% by mass or less.

[0038] Furthermore, from the viewpoint of further increasing the adhesive strength achieved by the adhesive layer, the proportion of aromatic vinyl monomer units in the polymer of the shell portion is preferably 50% by mass or more, more preferably 65% ​​by mass or more, and is preferably 99% by mass or less, more preferably 95% by mass or less, with all repeating units (all monomer units) contained in the polymer of the shell portion being 100% by mass.

[0039] The shell polymer may contain acid group-containing monomer units in addition to (meth)acrylic acid ester monomer units and aromatic vinyl monomer units. Examples of the acid group-containing monomer include monomers having an acid group, such as monomers having a carboxylic acid group, monomers having a sulfonic acid group, and monomers having a phosphoric acid group. Specifically, the acid group-containing monomer may be the same monomer as the acid group-containing monomer that can be used to form the core. Among these, the acid group-containing monomer is preferably a monomer having a carboxylic acid group, more preferably a monocarboxylic acid, and even more preferably (meth)acrylic acid. The acid group-containing monomer may be used alone or in combination of two or more types in any ratio. The proportion of the acid group-containing monomer units in the shell polymer is preferably 0.1% by mass or more, more preferably 0.4% by mass or more, and even more preferably 0.7% by mass or more, and is preferably 15% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, based on 100% by mass of all repeating units (total monomer units) contained in the shell polymer. By keeping the proportion of the acid group-containing monomer units within the above range, the dispersibility of the particulate polymer can be improved, and the adhesive strength achieved by the adhesive layer can be further increased.

[0040] Here, the polymer of the shell portion may contain a hydroxyl group-containing monomer unit. The proportion of the hydroxyl group-containing monomer unit in the polymer of the shell portion is preferably 0.1% by mass or more, more preferably 0.4% by mass or more, even more preferably 0.7% by mass or more, and preferably 15% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, based on 100% by mass of all repeating units (total monomer units) contained in the polymer of the shell portion. By keeping the proportion of the hydroxyl group-containing monomer unit within the above range, the dispersibility of the particulate polymer can be improved, and the adhesive strength achieved by the adhesive layer can be further increased.

[0041] The polymer of the shell portion may contain a crosslinkable monomer unit. Examples of the crosslinkable monomer include the same monomers as those exemplified as the crosslinkable monomers that can be used in the polymer of the core portion. Among these, di(meth)acrylic acid ester monomers and allyl methacrylate are preferred. The crosslinkable monomer may be used alone or in combination of two or more types in any ratio.

[0042] (Mass Proportion of Shell Portion to the Total of Core Portion and Shell Portion) In the particulate polymer having a core-shell structure, the mass proportion of the shell portion to the total of the core portion and shell portion is preferably 2 mass% or more, preferably 15 mass% or less, and more preferably 10 mass% or less. When the mass proportion of the shell portion is equal to or greater than the above lower limit, the inkjet ejection characteristics can be further improved. Furthermore, when the mass proportion of the shell portion is equal to or less than the above upper limit, the adhesive strength achieved by the adhesive layer can be further increased, and the secondary battery can exhibit even better battery characteristics. Here, the mass proportion of the shell portion to the total of the core portion and shell portion is determined from the ratio of the thickness of the core portion to the shell portion, which will be described later, and the specific gravity of the particulate polymer.

[0043] (Volume average particle diameter of particulate polymer having core-shell structure) The volume average particle diameter of the particulate polymer having a core-shell structure is preferably 100 nm or more, more preferably 200 nm or more, preferably 1500 nm or less, more preferably 900 nm or less, even more preferably 800 nm or less, and even more preferably 700 nm or less. If the volume average particle diameter of the particulate polymer having a core-shell structure is 100 nm or more, it is possible to suppress deterioration of battery characteristics due to an increase in the resistance of the secondary battery caused by blocking the lithium ion pathway in the substrate (electrode or separator). Furthermore, if the volume average particle diameter is 1500 nm or less, it is possible to further suppress nozzle clogging when the coating liquid is applied by an inkjet method, and it is possible to improve inkjet ejection characteristics.

[0044] (Method for preparing particulate polymer having core-shell structure) The particulate polymer having core-shell structure can be prepared, for example, by using the monomer of the polymer of core part and the monomer of the polymer of shell part, and polymerizing them step by step while changing the ratio of these monomers over time.Specifically, the particulate polymer can be prepared by a continuous multi-stage emulsion polymerization method and a multi-stage suspension polymerization method, in which the polymer of the previous stage is successively coated with the polymer of the subsequent stage.

[0045] Therefore, an example of obtaining a particulate polymer having the above core-shell structure by a multistage emulsion polymerization method will be described below.

[0046] For the polymerization, an emulsifier may be used in accordance with a conventional method, for example, an anionic surfactant such as sodium dodecylbenzenesulfonate or sodium dodecyl sulfate, a nonionic surfactant such as polyoxyethylene nonylphenyl ether or sorbitan monolaurate, or a cationic surfactant such as octadecylamine acetate. Furthermore, a polymerization initiator may be used, for example, a peroxide such as t-butylperoxy-2-ethylhexanoate, potassium persulfate, or cumene peroxide, or an azo compound such as 2,2'-azobis(2-methyl-N-(2-hydroxyethyl)-propionamide or 2,2'-azobis(2-amidinopropane) hydrochloride.

[0047] The polymerization procedure is as follows: first, a monomer for forming the core part and an emulsifier are mixed and emulsion-polymerized all at once to obtain a particulate polymer for forming the core part. Then, a monomer for forming the shell part is polymerized in the presence of the particulate polymer for forming the core part, thereby obtaining a particulate polymer having the above-mentioned core-shell structure.

[0048] In this case, when preparing a particulate polymer in which the outer surface of the core part is partially covered with the shell part, it is preferable to supply the monomer that forms the polymer for the shell part to the polymerization system in multiple divided portions or continuously. By supplying the monomer that forms the polymer for the shell part to the polymerization system in divided portions or continuously, the polymer that forms the shell part is formed in a particulate form, and this particle is bonded to the core part, thereby forming the shell part that partially covers the core part.

[0049] (Amount of particulate polymer having a core-shell structure) The amount of the particulate polymer having a core-shell structure in 100% by mass of the coating liquid of the present invention is preferably 3.0% by mass or more, more preferably 5.0% by mass or more, preferably 20.0% by mass or less, and more preferably 15% by mass or less. By having the amount of the particulate polymer having a core-shell structure within the above range, the coating liquid of the present invention having the desired dry matter elastic modulus distribution can be easily obtained. Furthermore, if the amount of the particulate polymer having a core-shell structure is equal to or greater than the above lower limit, the adhesiveness of the resulting adhesive layer can be further improved, and further, the decrease in adhesiveness due to repeated charge and discharge of the resulting secondary battery can be suppressed, and an increase in resistance in a cycle test can be suppressed. Furthermore, if the amount of the particulate polymer having a core-shell structure is equal to or less than the above upper limit, an increase in the internal resistance of the resulting secondary battery can be suppressed, and the output characteristics can be improved.

[0050] (Nonionic Surfactant) The coating liquid preferably contains a nonionic surfactant. If the coating liquid contains a nonionic surfactant, the adhesive layer can more firmly bond the battery components together, and the battery characteristics of the resulting secondary battery can be further improved. Examples of nonionic surfactants include, but are not limited to, compounds having a polyalkylene oxide structure such as ethylene oxide-propylene oxide copolymer, polyoxyalkylene alkyl ether, polyoxyalkylene alkylphenyl ether, polyethylene glycol fatty acid ester, and polyoxyethylene sorbitan fatty acid ester; sorbitan fatty acid ester; and glycerin fatty acid ester. Among these, from the viewpoints of increasing the adhesiveness of the resulting adhesive layer and reducing the internal resistance of the resulting nonaqueous secondary battery, it is preferable to use a compound having a polyalkylene oxide structure, and ethylene oxide-propylene oxide copolymer and polyoxyalkylene alkyl ether are preferred. In this specification, the term "polyalkylene oxide structure" refers to a structure in which alkylene oxide units such as ethylene oxide units and propylene oxide units are repeated two or more times.

[0051] The content of the nonionic surfactant is preferably 0.01% by mass or more, more preferably 0.03% by mass or more, and preferably 1.0% by mass or less, more preferably 0.5% by mass or less, and even more preferably 0.2% by mass or less, based on 100% by mass of the total mass of the coating liquid. If the content of the nonionic surfactant is equal to or greater than the lower limit, the adhesiveness of the resulting adhesive layer can be improved and the internal resistance of the resulting nonaqueous secondary battery can be reduced. Furthermore, if the content of the nonionic surfactant is equal to or less than the upper limit, inkjet coating can be performed satisfactorily.

[0052] (Optional Components) The coating liquid may contain optional components other than those described above. Examples of such optional components include a particulate polymer not having a core-shell structure, an anti-drying agent, and other optional additives.

[0053] Here, the glass transition temperature of the particulate polymer not having a core-shell structure is preferably -40°C or higher, more preferably -35°C or higher, even more preferably -30°C or higher, preferably 25°C or lower, more preferably less than 25°C, even more preferably 0°C or lower, even more preferably -10°C or lower, and even more preferably -20°C or lower. If the glass transition temperature of the particulate polymer not having a core-shell structure is -40°C or higher, the adhesiveness of the resulting adhesive layer can be improved. On the other hand, if the glass transition temperature of the particulate polymer not having a core-shell structure is 0°C or lower, detachment of components from the adhesive layer can be suppressed.

[0054] As the monomer used for preparing the particulate polymer that does not have a core-shell structure, the same monomer as the monomer exemplified as the monomer that can be used for producing the core polymer of the particulate polymer that has the core-shell structure can be mentioned.For example, as the monomer that can be used for preparing the particulate polymer that does not have a core-shell structure, it is preferable to use (meth)acrylic acid ester monomer, aromatic vinyl monomer, acid group-containing monomer, crosslinkable monomer, etc. Such monomers can be used alone or in combination of two or more kinds at any ratio.

[0055] From the viewpoint of enhancing the adhesiveness of the resulting adhesive layer, the proportion of (meth)acrylic acid ester monomer units in the particulate polymer not having a core-shell structure is preferably 40% by mass or more, more preferably 50% by mass or more, and even more preferably 60% by mass or more, and is preferably 85% by mass or less, more preferably 80% by mass or less, and even more preferably 75% by mass or less, with all repeating units (total monomer units) contained in the polymer being 100% by mass.

[0056] From the viewpoint of enhancing the adhesiveness of the resulting adhesive layer, the proportion of aromatic vinyl monomer units in the particulate polymer not having a core-shell structure is preferably 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more, with the total repeating units (total monomer units) contained in the polymer being 100% by mass, and is preferably 40% by mass or less, more preferably 35% by mass or less, and even more preferably 30% by mass or less.

[0057] The proportion of the acid group-containing monomer units in the particulate polymer having no core-shell structure is preferably 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 2% by mass or more, and is preferably 10% by mass or less, more preferably 7% by mass or less, and even more preferably 5% by mass or less, based on 100% by mass of all repeating units (total monomer units) contained in the polymer. By keeping the proportion of the acid group-containing units in the particulate polymer having no core-shell structure within the above range, the dispersibility of the particulate polymer can be improved.

[0058] From the viewpoint of further enhancing the adhesiveness of the adhesive layer, the proportion of crosslinkable monomer units in the particulate polymer not having a core-shell structure is preferably 0.2% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more, with the total repeating units (total monomer units) contained in the polymer being 100% by mass, and is preferably 5% by mass or less, more preferably 4% by mass or less, and even more preferably 3% by mass or less.

[0059] (Volume average particle diameter of particulate polymer not having core-shell structure) The volume average particle diameter of the particulate polymer not having a core-shell structure is preferably 50 nm or more, more preferably 100 nm or more, and even more preferably 200 nm or more, and is preferably 600 nm or less, more preferably 500 nm or less, and even more preferably 400 nm or less. If the volume average particle diameter of the particulate polymer not having a core-shell structure is within the above-mentioned range, the adhesiveness of the resulting adhesive layer can be improved.

[0060] (Content of particulate polymer not having a core-shell structure) The content of the particulate polymer not having a core-shell structure in the coating liquid can be appropriately adjusted within a range in which the desired effects of the present invention can be obtained, but it is preferably 1 part by mass or more, more preferably 5 parts by mass or more, per 100 parts by mass of the particulate polymer having a core-shell structure. When the content of the particulate polymer not having a core-shell structure is not less than the above lower limit, it is possible to suppress the particulate polymer from falling off from the substrate.

[0061] (Method for producing particulate polymer without core-shell structure) The particulate polymer without core-shell structure is not particularly limited, and can be prepared, for example, by polymerizing a monomer composition containing the above-mentioned monomer in an aqueous solvent such as water.Here, the ratio of each monomer in the monomer composition is usually the same as the ratio of each monomer unit in the particulate polymer without core-shell structure.The polymerization method and polymerization reaction are not particularly limited, and known polymerization methods and polymerization reactions can be used.

[0062] (Anti-drying Agent) As the anti-drying agent that may be contained in the coating liquid of the present invention, polyhydric alcohols are useful, and examples thereof include glycerin, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, 1,3-butanediol, 2,3-butanediol, etc. These may be used alone or in combination of two or more.

[0063] The content of the drying inhibitor in the coating liquid is preferably 4% or more, more preferably 8% or more, and is preferably 30% or less, more preferably 20% or less.

[0064] (Other Additives) Optional additives other than those described above include components such as a surface tension modifier, a dispersant different from the dispersant used in the polymerization, a viscosity modifier, a reinforcing material, and an electrolyte additive. These are not particularly limited as long as they do not affect the battery reaction, and known components can be used. These components may be used alone or in combination of two or more at any ratio.

[0065] (Dispersion Medium) The dispersion medium contained in the coating liquid of the present invention is not particularly limited, and examples thereof include water, substances commonly used as organic solvents, and mixtures thereof. Examples of organic solvents include, but are not limited to, cyclic aliphatic hydrocarbons such as cyclopentane and cyclohexane; aromatic hydrocarbons such as toluene and xylene; ketones such as ethyl methyl ketone and cyclohexanone; esters such as ethyl acetate, butyl acetate, γ-butyrolactone, and ε-caprolactone; nitriles such as acetonitrile and propionitrile; ethers such as tetrahydrofuran and ethylene glycol diethyl ether; and alcohols such as methanol, ethanol, isopropanol, ethylene glycol, propylene glycol, and ethylene glycol monomethyl ether. Among the above, water is preferred from the viewpoints of simplifying the equipment used and reducing the environmental impact. At least a portion of the dispersion medium can be removed by drying or the like during the manufacturing process of the adhesive layer.

[0066] (Method for preparing coating liquid) The method for preparing the coating liquid of the present invention is not particularly limited, and can be prepared, for example, by stirring and mixing the particulate polymer and any other optional components in the presence of a dispersion medium. Here, the stirring and mixing method is not particularly limited, and can be performed by a known method. Specifically, a general stirring vessel, ball mill, sand mill, bead mill, pigment disperser, ultrasonic disperser, crusher, homogenizer, planetary mixer, Filmix, etc. can be used. The mixing conditions are not particularly limited, and the mixing can usually be performed at a temperature in the range of room temperature to 80°C for 10 minutes to several hours.

[0067] (Method for manufacturing adhesive layer) The method for manufacturing an adhesive layer for a secondary battery of the present invention includes applying the coating liquid of the present invention by an inkjet method. Coating by the inkjet method can be performed using a known coating machine and employing a known operating method. The layer of the coating liquid provided by coating can be subjected to a process such as drying as necessary, thereby forming an adhesive layer.

[0068] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the following examples and can be implemented with any modifications within the scope of the claims of the present invention and their equivalents. In the following description, "%" and "parts" representing amounts are by weight unless otherwise specified. Furthermore, the operations described below were carried out under conditions of room temperature and normal pressure unless otherwise specified.

[0069] (Evaluation Method) (Glass Transition Temperature) A measurement sample was prepared by drying the aqueous dispersion of the particulate polymer prepared in each Production Example at a temperature of 130°C for 1 hour. 10 mg of the measurement sample was weighed into an aluminum pan, and measurement was carried out using a differential scanning calorimetry measuring device ("EXSTAR DSC6220" manufactured by SII NanoTechnology Inc.) at a temperature range of -100°C to 200°C at a heating rate of 10°C / min under the conditions specified in JIS Z8703 to obtain a differential scanning calorimetry (DSC) curve. An empty aluminum pan was used as a reference. During this heating process, the glass transition temperature (°C) was determined as the intersection point between the baseline immediately before the endothermic peak of the DSC curve where the differential signal (DDSC) was 0.05 mW / min / mg or more appeared and the tangent to the DSC curve at the first inflection point that appeared after the endothermic peak. For the particulate polymer having a core-shell structure, two peaks were detected, and the glass transition temperature of the core part of the particulate polymer was obtained based on the peak with the stronger intensity, and the glass transition temperature of the shell part of the particulate polymer was obtained based on the peak with the weaker intensity.

[0070] (Volume average particle diameter) The volume average particle diameter of the particulate polymer prepared in each production example was measured by a laser diffraction method. Specifically, an aqueous dispersion solution (solid content concentration 0.1 mass%) containing the prepared particulate polymer was used as a sample, and the volume average particle diameter D50 (nm) was determined as the particle diameter at which the cumulative volume calculated from the smallest diameter side became 50% in the particle size distribution (volume basis) obtained by a laser diffraction particle size distribution analyzer (manufactured by Beckman Coulter, Inc., product name "LS-13 320").

[0071] <Elastic Modulus Distribution> The coating liquid obtained in each of the Examples and Comparative Examples was weighed out onto an aluminum dish so that the solid content (components remaining after drying; components other than the dispersion medium) was 1.5±0.1 g, and dried at 25°C for at least 24 hours to obtain a dried coating liquid. Using a cryomicrotome (manufactured by Leica, product name "EM UC7+FC7"), the dried coating liquid was cut in a -100°C atmosphere so that the cross section was in the thickness direction to prepare 1 μm-thick slices. The slices were picked up on clean silicon wafers and used as measurement samples. Using an atomic force microscope (manufactured by Bruker, product name "Dimension Icon"), the elastic modulus of the measurement sample surface (cut surface) was measured with a silicon cantilever (manufactured by Olympus, product name "OMCL-AC240TS"). The measurement field of view was 5 μm × 5 μm. Measurements were performed at 16,384 points per field of view. The load applied by the cantilever to the surface of the measurement sample was 1 nN. The elastic modulus at each measurement point was calculated from the force curve obtained by the measurement. The number of measurement values ​​less than 5 MPa and the number of measurement values ​​equal to or greater than 5 MPa were counted from the 16,384 measurement points obtained, and the percentage of these numbers relative to the total number of measurement points was calculated as the proportion of the region less than 5 MPa and the proportion of the region equal to or greater than 5 MPa.

[0072] <Surface tension> The surface tension of the coating liquid obtained in each of the examples and comparative examples was measured by the platinum plate method using a high-performance surface tensiometer "DY-500" manufactured by Kyowa Interface Science Co., Ltd. The measurement was repeated three times. The average value of the three measured values ​​was calculated, and this average value was used as the surface tension of the coating liquid. This measurement was carried out at a measurement temperature of 30°C.

[0073] <Viscosity> The viscosity of the coating liquids obtained in each of the Examples and Comparative Examples was measured in accordance with JIS Z8803:1991 using a single cylindrical rotational viscometer (Brookfield B-type viscometer) under conditions of a rotation speed of 60 rpm and a temperature of 25°C.

[0074] <Intermittent Discharge Performance> The coating liquids obtained in each of the Examples and Comparative Examples were discharged using an inkjet type slurry supplying machine equipped with an inkjet head (Konica Corporation, product name "KM1024" (shear mode type)) under conditions that resulted in a flight speed of 6 to 10 m / sec, and then the discharge was stopped. The device was left for various periods of time that the discharge was stopped, and then the liquid was discharged again under the same conditions. The discharge stop period was set to various intervals of 5 minutes, such as 5 minutes, 10 minutes, 15 minutes, and so on, and the test was carried out. Nozzle clogging during the re-discharge was evaluated according to the following criteria.

[0075] A: Re-ejection was possible when left standing for up to 30 minutes or more. B: Re-ejection was possible up to 20 minutes, but when left standing for more than 20 minutes but less than 30 minutes, re-ejection was not possible due to nozzle clogging. C: Re-ejection was possible up to 10 minutes, but when left standing for more than 10 minutes but less than 20 minutes, re-ejection was not possible due to nozzle clogging. D: When left standing for 10 minutes or less, re-ejection was not possible due to nozzle clogging.

[0076] <Dry Adhesion Strength> A 5 ​​MPa pressure vessel equipped with a stirrer was charged with 33 parts of 1,3-butadiene, 3.5 parts of itaconic acid, 63.5 parts of styrene, 0.4 parts of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion-exchanged water, and 0.5 parts of potassium persulfate as a polymerization initiator. After thorough stirring, the mixture was heated to 50 ° C to initiate polymerization. When the polymerization conversion rate reached 96%, the mixture was cooled to terminate the reaction, yielding a mixture containing a binder (SBR) for the negative electrode composite layer. A 5% aqueous sodium hydroxide solution was added to the mixture containing the binder for the negative electrode composite layer, the pH was adjusted to 8, and unreacted monomer was removed by heated vacuum distillation. The mixture was then cooled to a temperature of 30 ° C or below to yield an aqueous dispersion containing the binder for the negative electrode composite layer.

[0077] Next, 100 parts of artificial graphite (volume average particle diameter: 15.6 μm) as the negative electrode active material, 1 part of a 2% aqueous solution of carboxymethylcellulose sodium salt (manufactured by Nippon Paper Industries Co., Ltd., product name "MAC350HC") as a viscosity modifier, in terms of solid content, and ion-exchanged water were mixed to adjust the solid content concentration to 68%, and then further mixed at a temperature of 25 ° C. for 60 minutes. Further, the solid content concentration was adjusted to 62% with ion-exchanged water, and then further mixed at a temperature of 25 ° C. for 15 minutes. To the obtained mixture, 1.5 parts of the aqueous dispersion containing the above-mentioned binder for the negative electrode composite layer, in terms of solid content, and ion-exchanged water were added, and the final solid content concentration was adjusted to 52%, and then further mixed for 10 minutes. This was degassed under reduced pressure to obtain a slurry composition for a secondary battery negative electrode with good fluidity.

[0078] The obtained secondary battery negative electrode slurry composition was applied to both sides of a 20 μm thick copper foil current collector using a comma coater so that the dried film thickness was approximately 150 μm, and then dried. This drying was performed by conveying the copper foil at a speed of 0.5 m / min through an oven at a temperature of 60 ° C for 2 minutes. Then, the copper foil was heat-treated at a temperature of 120 ° C for 2 minutes to obtain a pre-pressed negative electrode blank. This pre-pressed negative electrode blank was rolled using a roll press to obtain a negative electrode blank with a negative electrode composite layer thickness of 95 μm.

[0079] A polyethylene (PE) separator raw sheet (product name: "ND412" manufactured by Asahi Kasei, surface roughness (Sa): 0.2 μm) was prepared.

[0080] The coating liquid obtained in each of the Examples and Comparative Examples was supplied onto one surface of the negative electrode raw sheet from the inkjet head of an inkjet coating machine (Konica Corporation, KM1024 (shear mode type)). The supply was in the form of dots, and the supply basis weight (dry weight per unit area) was 0.1 g / m. 2 It was decided.

[0081] The negative electrode raw sheet and the separator raw sheet were overlapped with the coating layer sandwiched between them, and pressed with a press roll at a temperature of 50°C, a linear pressure of 20 kgf / cm, and a line speed of 1 m / min to obtain a laminate including a negative electrode, a dried coating layer, and a separator. The laminate was then cut out to obtain a large number of elongated rectangular test pieces measuring 25 mm x 60 mm.

[0082] The cellophane tape was fixed to a horizontal test table with the adhesive side facing up. The test specimen was attached to the cellophane tape with the negative electrode side facing down. The cellophane tape used was specified in JIS Z1522. One end of the separator in the longitudinal direction was pulled vertically upward at a pulling rate of 50 mm / min to peel it off, and the stress during peeling was measured.

[0083] This measurement was performed a total of six times, and the average stress was calculated and used as the peel strength. The peel strength was evaluated according to the following criteria. A higher peel strength indicates a higher dry adhesion between the electrode and the separator due to the dried product of the coating liquid.

[0084] A: Peel strength is 2.0 N / m or more. B: Peel strength is 1.0 N / m or more and less than 2.0 N / m. C: Peel strength is 0.5 N / m or more and less than 1.0 N / m. D: Peel strength is 0.1 N / m or more and less than 0.5 N / m.

[0085] (Production Example 1: Production of Particulate Polymer 1) (P1-1. Formation of Core Portion) 100 parts of ion-exchanged water and 0.3 parts of ammonium persulfate were supplied to a reactor equipped with a stirrer, the gas phase was replaced with nitrogen gas, and the temperature was raised to 80°C. Meanwhile, in a separate vessel, 40 parts of ion-exchanged water, 0.2 parts of sodium dodecylbenzenesulfonate as an emulsifier, 28.3 parts of styrene as an aromatic monovinyl monomer, 66.6 parts of 2-ethylhexyl acrylate as a monofunctional (meth)acrylic acid ester monomer, 3 parts of methacrylic acid as an acidic group-containing monomer, and 0.1 parts of ethylene glycol dimethacrylate as a crosslinkable monomer were mixed to obtain a monomer composition for forming a core portion. This monomer composition for forming a core portion was continuously added to the reactor over 3 hours, and a polymerization reaction was carried out at a temperature of 80°C. The polymerization was continued until the polymerization conversion rate reached 95%, thereby obtaining an aqueous dispersion containing a particulate polymer that constitutes the core portion.

[0086] (P1-2. Formation of shell portion) A monomer composition for forming a shell portion, which contained 1.3 parts of styrene as an aromatic monovinyl monomer, 0.65 parts of butyl acrylate, and 0.05 parts of methacrylic acid as an acidic group-containing monomer, was continuously supplied to the aqueous dispersion obtained in (P1-1) over 60 minutes, and polymerization was continued. When the polymerization conversion rate reached 98%, the reaction was stopped by cooling, thereby preparing an aqueous dispersion containing particulate polymer 1.

[0087] (P1-3. Evaluation) The volume average particle diameter D50 and glass transition temperature of the obtained particulate polymer 1 were measured. The results are shown in Table 1. In addition, by observing the cross-sectional structure of the particulate polymer using a transmission electron microscope (TEM), it was confirmed that the particulate polymer had a core-shell structure in which the shell part partially covers the outer surface of the core part.

[0088] (Production Example 2: Production of Particulate Polymer 2) To a 5 MPa pressure vessel equipped with a stirrer, 50 parts of methyl methacrylate and 25 parts of n-butyl acrylate as (meth)acrylic acid ester monomers for forming the core portion of the organic particles, 1 part of allyl methacrylate as a crosslinkable monomer, 4 parts of methacrylic acid as an acidic group-containing monomer, 1 part of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion-exchanged water, and 0.5 parts of potassium persulfate as a polymerization initiator were added, and after thorough stirring, the mixture was heated to 60 ° C. to initiate polymerization. When the polymerization conversion rate reached 96%, a mixture of 19 parts of styrene as an aromatic monovinyl monomer and 1 part of methacrylic acid as an acidic group-containing monomer for forming the shell portion of the organic particles was continuously added, and the mixture was heated to 70 ° C. to continue polymerization. When the polymerization conversion rate of all added monomers reached 96%, the mixture was cooled to stop the reaction, and an aqueous dispersion containing organic particles was obtained. The volume average particle diameter D50 and glass transition temperature of the obtained particulate polymer 2 were measured. The results are shown in Table 1. In addition, by observing the cross-sectional structure of the particulate polymer using a transmission electron microscope (TEM), it was confirmed that the particulate polymer had a core-shell structure in which the shell part partially covers the outer surface of the core part.

[0089] (Production Example 3: Production of Particulate Polymer 3) (P1-2) of Production Example 1 was not carried out, and the aqueous dispersion containing the particulate polymer constituting the core part obtained in (P1-1) was used as it was as an aqueous dispersion containing particulate polymer 3 having no core-shell structure. The volume average particle diameter D50 and glass transition temperature of the obtained particulate polymer 3 were measured. The results are shown in Table 1.

[0090] (Production Example 4: Production of Particulate Polymer 4) 90 parts of ion-exchanged water and 0.5 parts of ammonium persulfate were each supplied to a reactor equipped with a stirrer, the gas phase was replaced with nitrogen gas, and the temperature was raised to 80°C. Meanwhile, in a separate vessel, 15 parts of ion-exchanged water, 1.0 part of Neopelex G15 (manufactured by Kao Chemical Corporation) as an emulsifier, 70.0 parts of 2-ethylhexyl acrylate as a monofunctional (meth)acrylic acid ester monomer, 25.0 parts of styrene as an aromatic monovinyl monomer, 1.7 parts of allyl glycidyl ether and 0.3 parts of allyl methacrylate as crosslinkable monomers, and 3.0 parts of acrylic acid as an acidic group-containing monomer were mixed to obtain a monomer composition. This monomer composition was continuously added to the reactor over 4 hours to carry out polymerization. During the continuous addition, the reaction was carried out at a temperature of 80°C. After completion of the continuous addition, the mixture was further stirred at a temperature of 80°C for 3 hours to terminate the reaction. The obtained aqueous dispersion was cooled to a temperature of 25°C, and then an aqueous sodium hydroxide solution was added thereto to adjust the pH to 8.0. Thereafter, steam was introduced to remove unreacted monomers, thereby obtaining an aqueous dispersion of particulate polymer 4 not having a core-shell structure. The volume average particle diameter D50 and glass transition temperature of the obtained particulate polymer 4 were measured. The results are shown in Table 1.

[0091] An overview and evaluation results of Production Examples 1 to 4 are shown in Table 1. The meanings of the abbreviations in Table 1 are as follows: MMA: methyl methacrylate proportion (parts) BA: butyl acrylate proportion (parts) 2EHA: 2-ethylhexyl acrylate proportion (parts) St: styrene proportion (parts) MAA: methacrylic acid proportion (parts) AA: acrylic acid proportion (parts) AGE: allyl glycidyl ether proportion (parts) AMA: allyl methacrylate proportion (parts) EDMA: ethylene glycol dimethacrylate proportion (parts) Shell proportion: mass proportion (%) of the shell proportion in the total of the core and shell parts

[0092]

[0093] (Examples 1 to 4 and Comparative Examples 1 to 3) A particulate polymer, a surfactant, a dispersant, an anti-drying agent, and water were mixed in the proportions shown in Table 2 to prepare a coating liquid. As the particulate polymer, two types of particulate polymers A and C were used, or three types of particulate polymers A to C were used, as shown in Table 2. As particulate polymers A and B, particulate polymers 1 to 3 produced in Production Examples 1 to 3 were selected and used, as shown in Table 2. As particulate polymer C, particulate polymer 4 produced in Production Example 4 was used. As the surfactant, Noptex ED052 (manufactured by San Nopco Ltd.) was used. As the dispersant, a water-soluble acrylic acid-based dispersant (Aron (registered trademark) A-6114) was used. As the anti-drying agent, propylene glycol was used.

[0094] The obtained coating liquid was evaluated for the distribution of elastic modulus, surface tension at 30° C. and 50° C., viscosity, intermittent discharge performance, and dry adhesive strength. The results are shown in Table 2.

[0095]

[0096] *1: Dry adhesion was not achieved and measurements could not be performed.

[0097] From the above results, it is clear that the coating liquids of the examples can achieve both good inkjet intermittent ejection performance and high dry adhesive strength.

Claims

1. A coating liquid for a secondary battery, wherein a region in a cross section of a dried product of the coating liquid has an elastic modulus of 5 MPa or more as measured by observation with an atomic force microscope at room temperature is 5% or more and less than 50%.

2. The coating liquid according to claim 1, which has a surface tension at 30° C. of 30 mN / m or more and 50 mN / m or less.

3. The coating fluid according to claim 1, which contains adhesive particles, and part or all of said adhesive particles have a core-shell structure.

4. The coating liquid according to claim 3, wherein the adhesive particles other than the adhesive particles having a core-shell structure include particles having a glass transition temperature Tg of less than 25°C.

5. The coating liquid according to claim 1, comprising adhesive particles, the adhesive particles including particles having a glass transition temperature Tg of less than 25°C.

6. The coating liquid according to claim 1, which contains adhesive particles, the particle diameter of said adhesive particles being 100 nm or more and 1000 nm or less.

7. A method for producing an adhesive layer for a secondary battery, comprising applying the coating liquid according to any one of claims 1 to 6 by an inkjet method.

Citation Information

Patent Citations

  • Binder composition for nonaqueous secondary battery porous film, slurry composition for nonaqueous secondary battery porous film, and nonaqueous secondary battery porous film, nonaqueous secondary battery and production method therefor

    WO2018198940A1

  • Composition for nonaqueous secondary battery adhesive layer, battery member for nonaqueous secondary battery and manufacturing method of said battery member for nonaqueous secondary battery, as well as manufacturing method for laminate for nonaqeuous secondary battery, and manufacturing method for nonaqueous secondary battery

    WO2020045246A1

  • Multilayer body for nonaqueous secondary batteries, bonding composition, and nonaqueous secondary battery

    WO2022230621A1