Reflective mask blank, reflective mask, and manufacturing methods for reflective mask and semiconductor device
The reflective mask blank design with a higher crystallinity upper layer and lower layer improves adhesion and durability, addressing adhesion and durability issues in EUV lithography for high-power exposure sources.
Patent Information
- Application Number
- PCT/JP2024/008313
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-05
- Publication Date
- 2024-10-03
AI Technical Summary
In EUV lithography, the adhesion between thin film layers in reflective masks is insufficient, leading to defects, and high-power exposure light sources require thin films with higher durability.
A reflective mask blank with a multilayer reflective film and an absorber film, where the upper layer has higher crystallinity than the lower layer, and the difference in crystallite size between the two layers is 2 nm or more, improving adhesion and durability.
Enhances the adhesion between thin film layers, resulting in a reflective mask with improved durability and reduced defects, enabling effective pattern transfer in EUV lithography.
Smart Images

Figure JP2024008313_03102024_PF_FP_ABST
Abstract
Description
Reflective mask blank, reflective mask, and method for manufacturing reflective mask and semiconductor device
[0001] The present invention relates to a reflective mask used in the manufacture of semiconductor devices, a method for manufacturing the same, and a reflective mask blank used to manufacture the reflective mask. The present invention also relates to a method for manufacturing a semiconductor device using the reflective mask.
[0002] 2. Description of the Related Art In recent years, with the increasing demand for higher density and higher precision in VLSI devices, EUV lithography, an exposure technique using extreme ultraviolet (hereinafter referred to as EUV) light, has been proposed.
[0003] A reflective mask has a multilayer reflective film formed on a substrate to reflect exposure light, and an absorber pattern, which is a patterned absorber film formed on the multilayer reflective film to absorb the exposure light. In EUV lithography using a reflective mask, the light image reflected by the multilayer reflective film of the reflective mask is transferred onto a semiconductor substrate (transfer target) such as a silicon wafer through a reflective optical system. A reflective mask blank is used to manufacture a reflective mask.
[0004] As an example of a reflective mask, Patent Document 1 describes a reflective X-ray mask composed of an X-ray reflective film, an intermediate layer formed in a pattern, and an X-ray absorber layer. In the reflective X-ray mask of Patent Document 1, the etching selectivity between the intermediate layer and the X-ray absorber layer is 5 or more. Patent Document 1 also describes that the intermediate layer is made of a material containing chromium or titanium as a main component.
[0005] As an example of a reflective mask blank, Patent Document 2 describes a mask blank having, on a substrate, a reflective layer that reflects exposure light in a short wavelength range including the extreme ultraviolet region, a buffer layer for protecting the reflective layer during pattern formation on the absorber layer, and an absorber layer that absorbs the exposure light, in that order. Patent Document 2 also describes that the absorber layer has at least a two-layer structure, with a lower absorber layer composed of an absorber for exposure light in a short wavelength range including the extreme ultraviolet region, and an upper low-reflection layer composed of an absorber for inspection light used to inspect the mask pattern. Patent Document 2 also describes that the upper layer is made of a material containing tantalum (Ta), boron (B), and oxygen (O). Patent Document 2 also describes that the buffer layer is made of Cr or a substance mainly composed of Cr. Furthermore, Patent Document 2 describes that the reflectance to the inspection light decreases in the order of the multilayer reflective film surface, the buffer layer surface, and the absorber layer surface, and that the reflectance of the absorber layer surface to the wavelength of light used to inspect the pattern formed on the absorber layer is 20% or less.
[0006] JP-A-8-213303 Patent No. 4061319
[0007] The above-mentioned EUV lithography is an exposure technology that uses extreme ultraviolet light (EUV light). EUV light is light in the wavelength band of the soft X-ray region or vacuum ultraviolet region, and specifically light with a wavelength of about 0.2 to 100 nm. In the case of EUV lithography, EUV light with a wavelength of 13 to 14 nm (for example, a wavelength of 13.5 nm) can be used. In this specification, light includes not only visible light but also electromagnetic waves.
[0008] EUV lithography uses a reflective mask with an absorber pattern. EUV light irradiated onto the reflective mask is absorbed in areas where the absorber pattern is present and reflected in areas where the absorber pattern is not present. A multilayer reflective film (including a protective film) is exposed in areas where the absorber pattern is not present. The multilayer reflective film exposed on the surface of the reflective mask reflects the EUV light. In EUV lithography, the optical image reflected by the multilayer reflective film (areas where the absorber pattern is not present) is transferred onto a semiconductor substrate (transfer target) such as a silicon wafer through a reflection optical system.
[0009] The absorber pattern disposed on the multilayer reflective film of the reflective mask is formed by patterning the absorber film of the reflective mask blank. Furthermore, thin films other than the absorber film, such as a protective film and an etching mask film, may be disposed on the multilayer reflective film. Furthermore, the absorber film may be composed of multiple different layers (thin films). Therefore, multiple thin films, including at least the multilayer reflective film and the absorber film, are disposed on the substrate of the reflective mask blank.
[0010] When multiple different layers (thin films) are stacked on a substrate, if the adhesion at the interface between adjacent layers is insufficient, one layer may peel off from the other layer during the manufacturing process of the reflective mask blank and / or the manufacturing process of the reflective mask, resulting in defects.
[0011] Furthermore, when EUV lithography using a reflective mask is performed in a semiconductor manufacturing process, a light source (exposure light source) that generates EUV light with a short wavelength of around 13.5 nm is used to transfer a pattern formed on the reflective mask to a transfer target. In recent years, increasing the power of exposure light sources for EUV lithography has been considered. When a high-power exposure light source is used in EUV lithography, thin films such as pattern-forming thin films must have higher durability. Note that a high-power exposure light source can refer to an exposure light source with a power of, for example, 400 W or more.
[0012] Therefore, an object of the present invention is to provide a mask blank that can improve the adhesion between two layers of a thin film when the thin film includes two layers, and also to provide a reflective mask blank that has a thin film that can improve the adhesion between the two layers included in the thin film and has higher durability.
[0013] Another object of the present invention is to provide a reflective mask manufactured using the reflective mask blank, and a method for manufacturing a semiconductor device using the reflective mask.
[0014] In order to solve the above problems, the present invention has the following configuration.
[0015] (Structure 1) Structure 1 is a reflective mask blank comprising: a substrate; a multilayer reflective film provided on the substrate; and a thin film provided on the multilayer reflective film, wherein the thin film includes a lower layer and an upper layer provided on the lower layer, the lower layer is made of a material having an amorphous structure or a microcrystalline structure, and the upper layer has higher crystallinity than the lower layer.
[0016] (Configuration 2) Configuration 2 is the reflective mask blank of configuration 1, characterized in that the lower layer and the upper layer are in contact with each other.
[0017] (Configuration 3) Configuration 3 is the reflective mask blank according to configuration 1 or 2, characterized in that the thin film is an absorber film.
[0018] (Configuration 4) Configuration 4 is the reflective mask blank according to any one of configurations 1 to 3, wherein the difference between the crystallite size of the upper layer and the crystallite size of the lower layer is 2 nm or more.
[0019] (Structure 5) Structure 5 is the reflective mask blank according to any one of Structures 1 to 4, further comprising an etching mask film formed on the thin film in contact with the thin film, the etching mask film having lower crystallinity than the upper layer.
[0020] (Configuration 6) Configuration 6 is the reflective mask blank according to any one of configurations 1 to 5, further comprising a protective film between the multilayer reflective film and the thin film.
[0021] (Configuration 7) Configuration 7 is the reflective mask blank according to any one of configurations 1 to 6, wherein the lower layer and the upper layer are made of different materials.
[0022] (Structure 8) Structure 8 is the reflective mask blank according to any one of structures 1 to 7, wherein the upper layer contains at least one selected from Ag, Au, Pt, Pd, Ir, Re, Os, Ru, Ta, Cr, Ti, Nb, Mo, W, and Rh.
[0023] (Configuration 9) Configuration 9 is the reflective mask blank according to any one of configurations 1 to 8, wherein the crystallite size of the upper layer is greater than 3 nm.
[0024] (Structure 10) Structure 10 is a reflective mask comprising: a substrate; a multilayer reflective film provided on the substrate; and a thin film having a pattern provided on the multilayer reflective film, wherein the thin film includes a lower layer and an upper layer provided on the lower layer, the lower layer is made of a material having an amorphous structure or a microcrystalline structure, and the upper layer has higher crystallinity than the lower layer.
[0025] (Configuration 11) Configuration 11 is the reflective mask of configuration 10, wherein the lower layer and the upper layer are in contact with each other.
[0026] (Configuration 12) Configuration 12 is the reflective mask of configuration 10 or 11, wherein the thin film is an absorber film.
[0027] (Configuration 13) Configuration 13 is the reflective mask of any one of configurations 10 to 12, wherein the difference between the crystallite size of the upper layer and the crystallite size of the lower layer is 2 nm or more.
[0028] (Configuration 14) Configuration 14 is the reflective mask of any one of configurations 10 to 13, further comprising a protective film between the multilayer reflective film and the thin film.
[0029] (Configuration 15) Configuration 15 is the reflective mask of any one of configurations 10 to 14, wherein the lower layer and the upper layer are made of different materials.
[0030] (Configuration 16) Configuration 16 is the reflective mask of any one of Configurations 10 to 15, wherein the upper layer contains at least one selected from Ag, Au, Pt, Pd, Ir, Re, Os, Ru, Ta, Cr, Ti, Nb, Mo, W, and Rh.
[0031] (Configuration 17) Configuration 17 is the reflective mask of any one of configurations 10 to 16, wherein the crystallite size of the upper layer is greater than 3 nm.
[0032] (Configuration 18) Configuration 18 is a method for manufacturing a semiconductor device, comprising using a reflective mask formed by forming a pattern on the thin film of the reflective mask blank of any one of Configurations 1 to 9, or a reflective mask of any one of Configurations 10 to 17, to transfer the pattern to a transfer target on a semiconductor substrate.
[0033] According to the present invention, when a thin film includes two layers, a mask blank can be provided that can improve the adhesion between the two layers of the thin film.Furthermore, according to the present invention, a reflective mask blank can be provided that has a thin film that can improve the adhesion between the two layers included in the thin film and has higher durability.
[0034] Furthermore, according to the present invention, it is possible to provide a reflective mask manufactured using the reflective mask blank, and a method for manufacturing a semiconductor device using the reflective mask.
[0035] Fig. 1 is a cross-sectional view schematically showing an example of a reflective mask blank of the present embodiment. Fig. 2 is a cross-sectional view schematically showing another example of a reflective mask blank of the present embodiment. Fig. 3 is a cross-sectional view schematically showing an example of a method for manufacturing a reflective mask of the present embodiment. Fig. 4 is a cross-sectional view schematically showing an example of an EUV exposure apparatus.
[0036] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. Note that the following embodiments are intended to specifically explain the present invention, and are not intended to limit the scope of the present invention.
[0037] As shown in FIG. 1, this embodiment is a reflective mask blank 100 having a substrate 1, a multilayer reflective film 2 provided on the substrate 1, and a thin film provided on the multilayer reflective film.
[0038] FIG. 1 is a cross-sectional schematic diagram showing an example of a reflective mask blank 100 of this embodiment. The reflective mask blank 100 shown in FIG. 1 has a substrate 1, a multilayer reflective film 2 provided on the substrate 1, and a thin film provided on the multilayer reflective film 2. The thin film of the reflective mask blank 100 of this embodiment includes a lower layer and an upper layer provided on the lower layer. In the example shown in FIG. 1, the thin film is an absorber film 4, and the absorber film 4, which is the thin film of this embodiment, has a lower layer 42 and an upper layer 44. In this embodiment, a thin film having a predetermined lower layer and upper layer may be referred to as a "predetermined thin film."
[0039] The predetermined thin film of this embodiment can be any film formed on the multilayer reflective film 2. In the example shown in FIG. 1 , a protective film 3, an absorber film 4, and an etching mask film 6 are disposed on the multilayer reflective film 2. The predetermined thin film of this embodiment is preferably at least one selected from the protective film 3, the absorber film 4, and the etching mask film 6. In this case, the at least one thin film selected from the protective film 3, the absorber film 4, and the etching mask film 6 can be a predetermined thin film having a lower layer and an upper layer. The lower layer and the upper layer can be a pair of adjacent films as described above. That is, in the reflective mask blank 100 of this embodiment, the lower layer can be the protective film 3 and the upper layer can be the absorber film 4. In this case, the predetermined thin film is the protective film 3 as the lower layer and the absorber film 4 as the upper layer. Here, if the absorber film 4 is a stacked film including multiple layers, the upper layer of the predetermined thin film can be the layer of the absorber film 4 that is in contact with the protective film 3. Furthermore, in the reflective mask blank 100 of this embodiment, the lower layer can be the absorber film 4 and the upper layer can be the etching mask film 6. In this case, the predetermined thin film is the absorber film 4, which is the lower layer, and the etching mask film 6, which is the upper layer. Here, when the absorber film 4 is a laminated film including multiple layers, the lower layer of the predetermined thin film can be the layer of the multiple layers of the absorber film 4 that is in contact with the etching mask film 6.
[0040] Fig. 2 is a cross-sectional schematic diagram showing another example of a reflective mask blank 100 of this embodiment. The reflective mask blank 100 shown in Fig. 2 does not have an etching mask film 6. Furthermore, the reflective mask blank 100 of this embodiment may or may not have a protective film 3. The reflective mask blank 100 of this embodiment has at least a multilayer reflective film 2 and an absorber film 4 on a substrate 1. In the example shown in Fig. 2, the predetermined thin film is the absorber film 4, and the absorber film 4, which is the predetermined thin film of this embodiment, has a lower layer 42 and an upper layer 44.
[0041] The absorber film 4 is repeatedly exposed to cleaning solutions during the manufacturing process of a reflective mask blank, the manufacturing process of a reflective mask, and / or the manufacturing process of a semiconductor device using a reflective mask. Therefore, to reduce peeling of the absorber film 4 during the above processes, it is preferable that the absorber film 4 has high adhesion to films formed above and / or below the absorber film 4. Furthermore, when the absorber film 4 includes multiple layers, it is preferable that the multiple layers have high adhesion to each other. Therefore, it is preferable that the specified thin film of this embodiment includes at least a portion of the absorber film 4.
[0042] In the reflective mask blank 100 of this embodiment, the lower layer is made of a material having an amorphous structure or a microcrystalline structure, and the upper layer has higher crystallinity than the lower layer. The inventors discovered that when the lower and upper layers, which are two films (layers) arranged in contact with each other, have a predetermined crystallinity, the adhesion between the adjacent lower and upper layers can be improved, and predetermined thin films (upper and lower layers) with higher durability can be obtained, and arrived at the present invention.
[0043] The crystallinity of the upper and lower layers of a given thin film can be confirmed by X-ray diffraction (XRD). X-ray diffraction (XRD) of a given thin film or layer can be used to confirm whether the given thin film or layer has an amorphous structure or a microcrystalline structure. When a given thin film or layer has a crystalline structure or a microcrystalline structure, it can be said that the crystallinity is higher than when it has an amorphous structure. Here, the diffraction angle range for confirming crystallinity by X-ray diffraction (XRD) can be 30 degrees or more and 90 degrees or less.
[0044] When no distinguishable sharp peak is observed in the X-ray diffraction profile obtained by X-ray diffraction (XRD) of a predetermined thin film or layer, the predetermined thin film or layer can be determined to have an amorphous structure. Note that when the predetermined thin film or layer has a crystalline structure, a distinguishable sharp peak is observed in the X-ray diffraction profile obtained by XRD of the predetermined thin film or layer.
[0045] In this specification, when the maximum peak intensity Imax and the minimum intensity (background intensity) Imin in the X-ray diffraction profile (after fitting, which will be described later) are taken as Imax-Imin, a material having a ratio [Imax-Imin] / [Imax+Imin] of 0.15 or less is defined as microcrystalline (or amorphous).
[0046] In this specification, the phrase "the upper layer has higher crystallinity than the lower layer" means that the upper layer has a crystalline structure and the lower layer has an amorphous structure or a microcrystalline structure, or that the upper layer has a microcrystalline structure and the lower layer has an amorphous structure. When the upper layer has higher crystallinity than the lower layer, the crystallite size of the upper layer can be said to be larger than the crystallite size of the lower layer.
[0047] Furthermore, the crystallinity of a given thin film or layer can be determined by measuring the crystallite size of the given thin film or layer using X-ray diffraction (XRD). For example, in-plane measurement (2θχ / φ scan) can be used as the X-ray diffraction (XRD). A thin film or layer with a larger crystallite size can be said to have higher crystallinity than a thin film or layer with a smaller crystallite size.
[0048] The crystallite size of a predetermined thin film or layer can be determined as follows. That is, first, the profile of the diffraction angle range including the peak in the X-ray diffraction profile obtained by measuring the predetermined thin film or layer using the X-ray diffraction (XRD) method is fitted by the least squares method using the Gaussian function (Equation 1) below to obtain the diffraction angle u and σ. The crystallite size D can be determined from the diffraction angle u and the half-width β calculated from σ using the Scherrer formula (see Equation 2 below). The half-width β can be determined from the σ obtained by fitting using Equation 3 below. D = Kλ / β・cos(2 / u) (Formula 2)
[0049] In Equation 2, D is the crystallite size (nm), K is the Scherrer constant 0.9, λ is the wavelength of the X-ray (nm), and β is the half-width of the diffraction line (rad). 1) was set to a wavelength of 0.15405 (nm).
[0050] In addition, when there are multiple peaks observed in a given X-ray diffraction profile, the peak with the largest peak intensity or the peak with the largest peak area (the peak with the largest integrated intensity) can be selected, and the crystallite size can be determined from this peak. When there are multiple peaks with the largest peak intensity and / or the largest peak area and it is difficult to determine which peak to select, the peak with the smallest half-width can be selected from these multiple peaks.
[0051] The measurement range of the X-ray diffraction profile can be a 2θ range of 30 degrees to 90 degrees (θ range of 15 degrees to 45 degrees).
[0052] Furthermore, if no peak is observed in the X-ray diffraction profile, it can be determined that the measured thin film or layer has an amorphous structure.
[0053] In the reflective mask blank 100 of this embodiment, the difference between the crystallite size of the upper layer and the crystallite size of the lower layer is preferably 2 nm or more, more preferably 5 nm or more. This improves the adhesion of the upper layer to the lower layer. Furthermore, the crystallite size of the upper layer is preferably larger than 3 nm, more preferably larger than 8 nm. When the crystallite size of the upper layer is larger than a predetermined value, the adhesion of the upper layer to the lower layer can be improved. Furthermore, the crystallite size of the upper layer is preferably 20 nm or less, more preferably 19 nm or less, and even more preferably 18 nm or less. When the crystallite size of the upper layer is equal to or less than a predetermined value, the surface roughness of the predetermined thin film including the upper layer can be reduced, thereby obtaining a good thin film surface.
[0054] In the predetermined thin film included in the reflective mask blank 100 of this embodiment, the crystallinity of the upper layer is made high (the crystallite size is made large). Generally, when the crystallinity of a thin film is made high, the surface roughness of the thin film surface increases. On the other hand, in the predetermined thin film included in the reflective mask blank 100 of this embodiment, the crystallinity of the lower layer is made low by making the lower layer have an amorphous structure or a microcrystalline structure, so that the surface roughness of the predetermined thin film as a whole can be prevented from becoming too large.
[0055] In the reflective mask blank 100 of this embodiment, the etching rate of the upper layer can be increased by increasing the crystallinity of the upper layer of the predetermined thin film. On the other hand, the lower layer of the predetermined thin film of the reflective mask blank 100 of this embodiment has a relatively low crystallinity, e.g., the lower layer has an amorphous structure or a microcrystalline structure. Therefore, the lower layer can be more resistant to the etching gas of the upper layer. Furthermore, damage to the lower layer during etching of the upper layer can be reduced. This can further suppress damage to other thin films or layers (e.g., when the predetermined thin film is an absorber film 4, other thin films such as the multilayer reflective film 2 and / or the protective film 3) present further below the lower layer of the predetermined thin film (toward the substrate). As a result, the reflectivity of the multilayer reflective film 2 can be maintained high.
[0056] Generally, when patterning a thin film by etching, the larger the crystallite size, the easier it is for the etchant to penetrate into the thin film, resulting in an improved etching rate. In this embodiment, the crystallinity of the upper layer of a given thin film is high, so the etching rate of the upper layer can be improved. That is, by making the crystallite size of the upper layer in a given thin film larger than the crystallite size of the lower layer, the etching rate for etching a region within the given thin film can be made faster for the upper layer than for regions other than the upper layer. The longer the time required to etch the upper layer, the greater the possibility that films or layers other than the upper layer will be damaged. However, by using the above configuration, damage to films or layers other than the upper layer, such as the lower layer, can be suppressed.
[0057] The interplanar spacing of a predetermined lattice plane can be determined by Bragg's law from the diffraction angle of the X-ray diffraction profile of a predetermined layer obtained by the above-mentioned X-ray diffraction (XRD) method. The lattice plane can be one having Miller indices corresponding to the peak with the greatest peak intensity or the peak with the largest peak area (peak with the largest integrated intensity) within the diffraction angle range of 30 degrees to 90 degrees in the X-ray diffraction profile. When there are multiple peaks with the greatest peak intensity and / or the largest peak area and it is difficult to determine which peak to select, the peak with the smallest half-width among these multiple peaks can be selected. The lattice spacing d of the upper layer obtained by the XRD method is preferably 0.27 nm or less, more preferably 0.25 nm or less, and even more preferably 0.23 nm or less. This can prevent oxygen with a kinetic molecular diameter of 0.346 nm and hydrogen with a kinetic molecular diameter of 0.289 nm from penetrating the predetermined thin film. As a result, damage and / or deterioration of the predetermined thin film can be suppressed.
[0058] In the reflective mask blank of this embodiment, the lower and upper layers of the predetermined thin film are preferably made of different materials. By making the lower and upper layers of the predetermined thin film from different materials, it becomes easier to control the lower and upper layers so that they have predetermined crystallinity. Furthermore, the selectivity with respect to the etching gas when etching the lower and upper layers can be made appropriate.
[0059] In the reflective mask blank of this embodiment, the lower layer and the upper layer are preferably in contact with each other, which can improve the adhesion between the adjacent lower and upper layers and provide a predetermined thin film (upper and lower layers) with higher durability.
[0060] 1 and 2 may further include other thin films such as a back surface conductive film 5. Furthermore, as shown in FIG. 3A, the reflective mask blank 100 of this embodiment may further include a resist film 11.
[0061] In this specification, "disposing (forming) film B on film A (or substrate)" not only means that film B is disposed (formed) in contact with the surface of film A (or substrate), but also means that another film C is present between film A (or substrate) and film B. Furthermore, in this specification, for example, "disposing film B in contact with the surface of film A (or substrate)" means that film A (or substrate) and film B are disposed so as to be in direct contact with each other, without any other film interposed between them. Furthermore, in this specification, "above" does not necessarily mean above in the vertical direction. "Above" merely indicates the relative positional relationship between a film, a substrate, etc. In this embodiment, when two films, film A and film B, exist in the reflective mask blank 100, if film A is disposed farther from the substrate than film B, it is said that "film A is above (disposed) film B." In this embodiment, the upper layer of the reflective mask blank 100 is provided on the lower layer, and therefore the upper layer is disposed farther from the substrate than the lower layer.
[0062] In the reflective mask blank 100 of this embodiment, the predetermined thin film is preferably an absorber film 4. In the case of an absorber film 4, multiple layers may be formed to improve performance. As a result, there is a risk that defects may occur due to film peeling due to a decrease in adhesion between the multiple layers included in the absorber film 4. The reflective mask blank 100 of this embodiment can improve the adhesion between the multiple layers included in the absorber film 4, making it possible to manufacture a reflective mask having an absorber film 4 that is less prone to defects and has higher durability.
[0063] The above explanation uses a reflective mask blank 100 for manufacturing a reflective mask as an example, but the specified thin films (lower and upper layers) of this embodiment can also be applied to mask blanks other than reflective mask blanks (e.g., binary mask blanks and phase-shift mask blanks).
[0064] <Reflective Mask Blank 100> The reflective mask blank 100 of this embodiment will be specifically described. Hereinafter, the case where the predetermined thin film is an absorber film 4 and the absorber film 4, which is the predetermined thin film of this embodiment, has a lower layer 42 and an upper layer 44 will be described as an example.
[0065] <<Substrate 1>> The substrate 1 is preferably made of a material having a low thermal expansion coefficient within the range of 0±5 ppb / °C in order to prevent distortion of the transferred pattern due to heat during exposure to EUV light. Examples of materials having a low thermal expansion coefficient within this range include SiO 2 -TiO 2 Glasses and multi-component glass ceramics can be used.
[0066] The main surface (first main surface) of the substrate 1 on which a transfer pattern (the absorber pattern 4a described below) is formed is preferably processed to increase its flatness. Increasing the flatness of the main surface of the substrate 1 can improve the positional accuracy and transfer accuracy of the pattern. For example, in the case of EUV exposure, the flatness in a 132 mm × 132 mm area of the main surface of the substrate 1 on which the transfer pattern is formed is preferably 0.1 μm or less, more preferably 0.05 μm or less, and particularly preferably 0.03 μm or less. Furthermore, the second main surface (rear surface) opposite the side on which the transfer pattern is formed is the surface fixed to the exposure apparatus by an electrostatic chuck. In a 142 mm × 142 mm area of the rear surface, the flatness is 0.1 μm or less, more preferably 0.05 μm or less, and particularly preferably 0.03 μm or less. In this specification, flatness is a value representing the warpage (deformation) of the surface indicated by TIR (Total Indicated Reading). The flatness (TIR) is the absolute value of the difference in height between the highest point on the surface of substrate 1 above the focal plane, which is determined by the least squares method using the surface of substrate 1 as a reference, and the lowest point on the surface of substrate 1 below this focal plane.
[0067] In the case of EUV exposure, the surface roughness of the main surface of the substrate 1 on which the transfer pattern is formed is preferably 0.1 nm or less in terms of root mean square roughness (Rq). The surface roughness can be measured using an atomic force microscope.
[0068] The substrate 1 preferably has high rigidity to prevent deformation due to film stress of the thin films (such as the multilayer reflective film 2) formed thereon. In particular, the substrate 1 preferably has a high Young's modulus of 65 GPa or more.
[0069] <<Multilayer reflective film 2>>
[0070] The reflective mask blank 100 of the embodiment includes a multilayer reflective film 2. The multilayer reflective film 2 provides the reflective mask 200 with the function of reflecting EUV light. The multilayer reflective film 2 is a multilayer film in which layers each containing materials with different refractive indices as main components are periodically stacked.
[0071] Generally, the multilayer reflective film 2 is a multilayer film in which thin films of high refractive index materials, i.e., light elements or compounds thereof (high refractive index layers), and thin films of low refractive index materials, i.e., heavy elements or compounds thereof (low refractive index layers), are alternately stacked in approximately 30 to 60 cycles.
[0072] The multilayer film used as the multilayer reflective film 2 can have a structure in which multiple cycles of a high-refractive-index layer / low-refractive-index layer stacked in this order from the substrate 1 side are stacked. Alternatively, the multilayer film can have a structure in which multiple cycles of a low-refractive-index layer / high-refractive-index layer stacked in this order from the substrate 1 side are stacked. The topmost layer of the multilayer reflective film 2, i.e., the surface layer of the multilayer reflective film 2 opposite the substrate 1 side, is preferably a high-refractive-index layer. In the above-described multilayer film, when multiple cycles of a high-refractive-index layer / low-refractive-index layer stacked in this order from the substrate 1 side are stacked, the topmost layer is the low-refractive-index layer. In this case, if the low-refractive-index layer constitutes the topmost surface of the multilayer reflective film 2, it will be easily oxidized, potentially reducing the reflectivity of the reflective mask 200. Therefore, it is preferable to form the multilayer reflective film 2 by further forming a high-refractive-index layer on the topmost low-refractive-index layer. On the other hand, in the above-mentioned multilayer film, when a low-refractive index layer / high-refractive index layer stack structure in which a low-refractive index layer and a high-refractive index layer are stacked in this order from the substrate 1 side is defined as one cycle, and multiple cycles are stacked, the uppermost layer is the high-refractive index layer, and therefore, in this case, there is no need to form an additional high-refractive index layer.
[0073] The high-refractive index layer can be a layer containing silicon (Si). Examples of materials containing Si include elemental Si and Si compounds containing boron (B), carbon (C), nitrogen (N), oxygen (O), and / or hydrogen (H). By using a high-refractive index layer containing Si, a reflective mask 200 with excellent EUV light reflectivity can be obtained. The low-refractive index layer can be a metal element selected from molybdenum (Mo), ruthenium (Ru), rhodium (Rh), and platinum (Pt), or an alloy thereof. These metal elements or alloys may be doped with boron (B), carbon (C), nitrogen (N), oxygen (O), and / or hydrogen (H). In the reflective mask blank 100 of this embodiment, the low-refractive index layer is preferably a molybdenum (Mo) layer, and the high-refractive index layer is preferably a silicon (Si) layer. For example, as a multilayer reflective film 2 for reflecting EUV light with a wavelength of 13 nm to 14 nm (e.g., a wavelength of 13.5 nm), a Mo / Si periodic stacked film in which Mo layers and Si layers are alternately stacked for approximately 30 to 60 periods can be preferably used. Furthermore, in the reflective mask blank 100 of this embodiment, the low refractive index layers may be ruthenium (Ru) layers, and the high refractive index layers may be silicon (Si) layers. For example, as a multilayer reflective film 2 for reflecting EUV light with a wavelength of 13 nm to 14 nm (e.g., a wavelength of 13.5 nm), a Ru / Si periodic stacked film in which Ru layers and Si layers are alternately stacked for approximately 30 to 40 periods can be preferably used.
[0074] The reflectivity of the multilayer reflective coating 2 can be 65% or more, and the upper limit can be 73%. The reflectivity in this specification refers to the value when the angle of incidence of EUV light with respect to the multilayer reflective coating 2 (including the protective coating 3) is the same as the angle of incidence of EUV light with respect to the target to be irradiated, which is used in exposure when a pattern is transferred using the reflective mask 200 or a reflective mask 200 manufactured from the reflective mask blank 100. When transferring a pattern, EUV light from the EUV light source is irradiated onto the reflective mask 200 via an illumination optical system at an angle tilted, for example, by 6 to 8 degrees, with respect to a plane perpendicular to the main surface of the reflective mask 200. The angle of incidence of EUV light with respect to the multilayer reflective coating 2 is not particularly limited, but can be, for example, 6 degrees.
[0075] The thickness and period of each constituent layer of the multilayer reflective film 2 can be appropriately selected depending on the exposure wavelength. Specifically, the thickness and period of each constituent layer of the multilayer reflective film 2 can be selected so as to satisfy the law of Bragg reflection. The multilayer reflective film 2 includes a plurality of high refractive index layers and a plurality of low refractive index layers, but the thicknesses of the high refractive index layers and the low refractive index layers do not necessarily have to be the same.
[0076] Methods for forming the multilayer reflective film 2 are known in the art. The multilayer reflective film 2 can be formed by depositing each layer by, for example, ion beam sputtering. In the case of the Mo / Si periodic multilayer film described above, for example, an Si film having a thickness of about 4 nm is first deposited on the substrate 1 using a Si target by ion beam sputtering or magnetron sputtering, and then an Mo film having a thickness of about 3 nm is deposited using a Mo target. This constitutes one period, and 30 to 60 periods are stacked to form the multilayer reflective film 2 (the outermost layer is a Si film). Note that, although 60 periods requires more steps than 30 periods, the reflectivity for EUV light can be increased.
[0077] <<Protective film 3>> The reflective mask blank 100 of this embodiment preferably includes a protective film 3 between the multilayer reflective film 2 and the absorber film 4 described below. The protective film 3 is arranged in contact with the surface of the multilayer reflective film 2 opposite the substrate 1. When the reflective mask blank 100 includes the protective film 3, the reflected light of the multilayer reflective film 2 refers to light that is incident on the multilayer reflective film 2 via the protective film 3 and is reflected via the protective film 3. In other words, when the reflective mask blank 100 includes the protective film 3, the reflected light from the surface of the protective film 3 in a state in which the protective film 3 is formed on the multilayer reflective film 2 on the substrate 1 may be measured as the reflected light of the multilayer reflective film 2.
[0078] In the reflective mask blank 100 of this embodiment, the protective film 3 is formed between the multilayer reflective film 2 and the absorber film 4, thereby making it possible to suppress damage to the surface of the multilayer reflective film 2 when manufacturing a reflective mask 200 (EUV mask) using the reflective mask blank 100. As a result, the resulting reflective mask 200 has good reflectance characteristics for EUV light.
[0079] The protective film 3 preferably contains at least one selected from ruthenium (Ru), rhodium (Rh), and iridium (Ir). The protective film 3 more preferably contains at least one selected from ruthenium (Ru) and rhodium (Rh). The protective film 3 may further contain an additive element in addition to the above elements. The additive element contained in the protective film 3 is preferably one or more elements selected from Tl, Hf, Ti, Zr, Mn, In, Ga, Cd, Bi, Ta, Pb, Ag, Al, V, Nb, Sn, Zn, Hg, Cr, Fe, Sb, W, Mo, and Cu.
[0080] The Ru content of the protective film 3 is 50 atomic % or more and less than 100 atomic %, preferably 80 atomic % or more and less than 100 atomic %, and more preferably 95 atomic % or more and less than 100 atomic %. The Rh content is 10 atomic % or more and less than 70 atomic %, preferably 20 atomic % or more and less than 60 atomic %, and more preferably 30 atomic % or more and less than 50 atomic %. In this case, the protective film 3 can be provided with sufficient reflectivity for EUV light, mask cleaning resistance, an etching stopper function when the absorber film 4 is etched, and a function of preventing deterioration of the multilayer reflective film 2 over time.
[0081] The protective film 3 may also have a laminated structure of two or more layers.
[0082] Furthermore, in the reflective mask blank 100 of this embodiment, an underlayer may be formed between the substrate 10 and the multilayer reflective film 2. The underlayer can be formed for the purposes of improving the smoothness of the main surface of the substrate 10, reducing defects, enhancing the reflectivity of the multilayer reflective film 2, and correcting stress in the multilayer reflective film 2.
[0083] <<Backside Conductive Film 5>> The reflective mask blank 100 of this embodiment can have a backside conductive film 5 for electrostatic chucks. The backside conductive film 5 can be formed on the second main surface (backside) of the substrate 1. The second main surface is the main surface opposite to the surface on which the multilayer reflective film 2 is formed. If an intermediate layer such as a hydrogen penetration suppression film is formed on the second main surface of the substrate 1, the backside conductive film 5 can be formed on the intermediate layer. The sheet resistance required for the backside conductive film 5 for electrostatic chucks is typically 100 Ω / □ (Ω / square) or less. The backside conductive film 5 can be formed by, for example, magnetron sputtering or ion beam sputtering using a target of a metal such as chromium or tantalum, or an alloy thereof. The chromium (Cr)-containing material of the backside conductive film 5 is preferably a Cr compound containing Cr and at least one element selected from boron, nitrogen, oxygen, and carbon. Examples of Cr compounds include CrN, CrON, CrCN, CrCON, CrBN, CrBON, CrBCN, and CrBOCN. The tantalum (Ta)-containing material of the backside conductive film 5 is preferably Ta (tantalum), a Ta-containing alloy, or a Ta compound containing at least one of boron, nitrogen, oxygen, and carbon. Examples of Ta compounds include TaB, TaN, TaO, TaON, TaCON, TaBN, TaBO, TaBON, TaBCON, TaHf, TaHfO, TaHfN, TaHfON, TaHfCON, TaSi, TaSiO, TaSiN, TaSiON, and TaSiCON. The thickness of the back surface conductive film 5 is not particularly limited as long as it satisfies the function of the electrostatic chuck, but is usually 10 nm to 200 nm. The back surface conductive film 5 also serves to adjust the stress on the second main surface side of the mask blank 100. That is, the back surface conductive film 5 is adjusted to achieve a balance with the stress from the various films formed on the first main surface side, so as to obtain a flat reflective mask blank 100.
[0084] It should be noted that the reflective mask blank 100 does not necessarily need to include the back surface conductive film 5. For example, the back surface conductive film 5 can be formed, if necessary, on the reflective mask blank 100 on which the absorber film 4 described below has been formed.
[0085] 1 and 2 , the absorber film 4 of the reflective mask blank 100 of this embodiment is disposed on the above-mentioned multilayer reflective film 2. When the reflective mask blank 100 includes a protective film 3, the absorber film 4 is disposed on the protective film 3. The absorber film 4 can be disposed in contact with the surface of the protective film 3. When the reflective mask blank 100 does not include a protective film 3, the absorber film 4 can be disposed in contact with the surface of the multilayer reflective film 2.
[0086] The basic function of the absorber film 4 is to absorb EUV light. The absorber film 4 may be an absorber film 4 intended for absorbing EUV light, or an absorber film 4 having a phase shift function that also takes into account the phase difference of EUV light. An absorber film 4 having a phase shift function absorbs EUV light and reflects a portion of it to shift its phase. That is, in a reflective mask 200 patterned with an absorber film 4 having a phase shift function, the portion where the absorber film 4 is formed absorbs and attenuates EUV light while reflecting a portion of the light at a level that does not adversely affect pattern transfer. Furthermore, in regions (field portions) where the absorber film 4 is not formed, the EUV light is reflected from the multilayer reflective film 2 (via the protective film 3, if present). Therefore, a desired phase difference is generated between the light reflected from the absorber film 4 having a phase shift function and the light reflected from the field portion. The absorber film 4 having a phase shift function is formed so that the phase difference between the reflected light from the absorber film 4 and the reflected light from the multilayer reflective film 2 is 100 to 310 degrees. The phase difference is preferably 150 degrees or more, more preferably 180 degrees or more, and even more preferably 200 degrees or more. The phase difference is preferably 300 degrees or less, more preferably 280 degrees or less, and even more preferably 250 degrees or less. Light beams with inverted phase differences interfere with each other at the pattern edge, improving the image contrast of the projected optical image. This improvement in image contrast increases resolution, and various exposure latitudes, such as exposure dose latitude and focus latitude, can be increased.
[0087] In the reflective mask blank 100 of this embodiment, the predetermined thin film is preferably an absorber film 4 .
[0088] 1 and 2, the absorber film 4 (predetermined thin film) of the reflective mask blank 100 of this embodiment can include a lower layer 42 and an upper layer 44. The lower layer 42 is disposed between the upper layer 44 and the multilayer reflective film 2 (or between the upper layer 44 and the protective film 3 if the protective film 3 is present). The absorber film 4 can include films other than the lower layer 42 and the upper layer 44. The reflective mask blank 100 of this embodiment has the absorber film 4, which is a predetermined thin film, so that the adhesion between the two layers (the lower layer 42 and the upper layer 44) included in the absorber film 4 can be improved.
[0089] In the reflective mask blank 100 of this embodiment, the lower layer 42 and the upper layer 44 are preferably in contact with each other. By having the lower layer 42 and the upper layer 44 in contact with each other, it is possible to reliably improve the adhesion between the lower layer 42 and the upper layer 44.
[0090] The lower layer 42 of the absorber film 4 can be a buffer layer. The buffer layer of the absorber film 4 is a layer disposed in contact with the protective film 3 and serves to suppress adverse effects on the protective film 3 when the absorber film 4 is etched to form the absorber pattern 4a. Specifically, a material that can be etched using an etching gas that does not damage the protective film 3 can be used as the material for the lower layer 42. In this case, although there is a risk of damage to the protective film 3 when etching the upper layer 44, an etching gas that has a high etching rate for the upper layer 44 can be used. Therefore, by including the lower layer 42, which is a buffer layer, and the upper layer 44 in the absorber film 4, the etching time for the absorber film 4 can be shortened, and adverse effects on the protective film 3 can be suppressed when the absorber film 4 is etched to form the absorber pattern 4a.
[0091] Specifically, if the protective film 3 is made of a material containing ruthenium (Ru) and the absorber film 4 is also made of a material containing ruthenium (Ru) (e.g., PtRu), both the protective film 3 and the absorber film 4 will be etched with a fluorine-based etching gas. In this case, etching the absorber film 4 to form the absorber pattern 4a may have an adverse effect on the protective film 3. Therefore, by configuring the absorber film 4 to include an upper layer 44 and a lower layer 42, with the lower layer 42 functioning as a buffer layer, the adverse effect on the protective film 3 can be suppressed. In this case, the material for the buffer layer, which is the lower layer 42, can be a material that is etch-resistant to a fluorine-based etching gas. For example, the material for the buffer layer, which is the lower layer 42, can be a material that can be etched with a chlorine-based etching gas.
[0092] The lower layer 42 of the reflective mask blank 100 of this embodiment is made of a material containing an amorphous structure or a microcrystalline structure. The upper layer 44 of the reflective mask blank 100 of this embodiment has higher crystallinity than the lower layer 42.
[0093] When the predetermined thin film of the reflective mask blank 100 of this embodiment is an absorber film 4, the lower layer 42 of the absorber film 4 is made of a material having an amorphous structure or a microcrystalline structure. Furthermore, the crystallinity of the upper layer 44 of the absorber film 4 is higher than that of the lower layer 42. When the lower layer 42 and the upper layer 44 arranged in contact with each other have a predetermined crystallinity, the adhesion between the adjacent lower layer 42 and upper layer 44 can be improved. Furthermore, by using the reflective mask blank 100 of this embodiment having a predetermined absorber film 4, an absorber pattern 4a with higher durability can be obtained.
[0094] In the reflective mask blank 100 of this embodiment, the crystallite size of the upper layer 44 of the absorber film 4 is preferably larger than 3 nm, and more preferably larger than 8 nm. When the crystallite size of the upper layer 44 of the absorber film 4 is larger than a predetermined value, the adhesion of the absorber film 4 to the lower layer 42 can be improved. Furthermore, the crystallite size of the upper layer 44 of the absorber film 4 is preferably 20 nm or less, more preferably 19 nm or less, and even more preferably 18 nm or less. When the crystallite size of the upper layer 44 of the absorber film 4 is a predetermined value or less, the surface roughness of the absorber film 4 including the upper layer 44 can be made good.
[0095] By increasing the crystallite size of the upper layer 44 of the absorber film 4, the etching rate of the upper layer 44 can be increased. On the other hand, in the reflective mask blank 100 of this embodiment, the lower layer 42 of the absorber film 4 has relatively low crystallinity. For example, the lower layer 42 has an amorphous structure or a microcrystalline structure. Therefore, the lower layer 42 can be more resistant to the etching gas of the upper layer 44, and damage to the lower layer 42 during etching of the upper layer 44 can be reduced. Therefore, damage to other films (e.g., the multilayer reflective film 2 and / or the protective film 3) present further below the lower layer 42 of the absorber film 4 (toward the substrate 1) can be further suppressed. As a result, the reflectivity from the multilayer reflective film 2 can be maintained high.
[0096] The lattice spacing of a predetermined lattice plane can be determined from the diffraction angles of X-rays from the upper layer 44 and the lower layer 42 of the absorber film 4 obtained by the X-ray diffraction (XRD) method. As described above, the lattice plane can be one having Miller indices corresponding to the peak with the greatest peak intensity or the peak with the largest peak area (peak with the largest integrated intensity) within the diffraction angle range of 30 degrees to 90 degrees in the X-ray diffraction profile. When there are multiple peaks with the greatest peak intensity and / or the largest peak area and it is difficult to determine which peak to select, the peak with the smallest half-width among these multiple peaks can be selected. The lattice spacing d of the upper layer 44 of the absorber film 4 obtained by the XRD method is preferably 0.27 nm or less, more preferably 0.25 nm or less, and even more preferably 0.23 nm or less. This prevents oxygen with a kinetic molecular diameter of 0.346 nm and hydrogen with a kinetic molecular diameter of 0.289 nm from penetrating the absorber film 4. As a result, damage and / or deterioration of the absorber film 4 can be suppressed.
[0097] According to the findings of the present inventors, the correlation between the high crystallinity and the high density of the film is considered to be low. Also, the correlation between the crystallite size and the film density is considered to be low. Therefore, it cannot be said that the film density is necessarily high when the crystallinity is high or the crystallite size is large.
[0098] In the reflective mask blank 100 of this embodiment, the lower layer 42 and the upper layer 44 of the absorber film 4 are preferably made of different materials. By making the lower layer 42 and the upper layer 44 of the absorber film 4 different materials, it becomes easier to control the lower layer 42 and the upper layer 44 to have predetermined crystallinity. Furthermore, by making the lower layer 42 and the upper layer 44 of the absorber film 4 different materials, it is possible to make the selectivity with respect to the etching gas when etching the lower layer 42 and the upper layer 44 appropriate.
[0099] The lower layer 42 of the absorber film 4 is preferably made of a material that can protect the multilayer reflective film 2 and / or the protective film 3 when the upper layer 44 of the absorber film 4 is etched.
[0100] The lower layer 42 of the absorber film 4 is not particularly limited as long as it is amorphous or microcrystalline and has a crystallite size smaller than that of the upper layer 44. For example, the material of the lower layer 42 of the absorber film 4 can be a material containing at least one selected from Ta, Cr, Ru, Rh, Mo, Nb, Ti, Zr, Y, Si, Pd, Ag, Ir, W, Co, Mn, Sn, V, Ni, Fe, Hf, Cu, Te, Zn, Mg, Ge, and Al. The material of the lower layer 42 of the absorber film 4 can further contain at least one selected from O, N, C, and B. Specific examples of the lower layer 42 of the absorber film 4 include Cr-based materials, Ta-based materials, Ru-based materials, RuCr materials, and RuTa materials, as well as materials further containing at least one selected from O, N, C, and B.
[0101] The material of the upper layer 44 of the absorber film 4 is not particularly limited as long as it can make the crystallinity of the upper layer 44 higher than that of the lower layer 42. Examples of materials for the upper layer 44 of the absorber film 4 include materials containing at least one selected from Ru, Ta, Cr, Rh, Mo, Nb, Ti, Zr, Y, Si, Pd, Ag, Pt, Au, Ir, W, Co, Mn, Sn, V, Ni, Fe, Hf, Cu, Te, Zn, Mg, Ge, Al, Au, Re, Os, and Rn. The material of the upper layer 44 of the absorber film 4 can further contain at least one selected from N, O, C, B, and H.
[0102] In order to obtain an absorber film 4 having a high extinction coefficient for EUV light, the upper layer 44 of the absorber film 4 preferably contains at least one selected from Ag, Au, Pt, Pd, Ir, Re, Os, Ru, Ta, Cr, Ti, Nb, Mo, W, and Rh. The upper layer 44 of the absorber film 4 may further contain at least one selected from N, O, C, B, and H. In particular, a material containing Pt and / or Ru is useful for obtaining a phase shift film (absorber film 4) having a high extinction coefficient for EUV light and a low refractive index.
[0103] When the upper layer 44 of the absorber film 4 is made of a material containing Pt and Ru, the material of the lower layer 42 and / or the etching mask film 6 is preferably a Cr-based material or a Ta-based material. The material of the lower layer 42 and / or the etching mask film 6 is preferably a material that further contains at least one element selected from O, N, C, and B in addition to the above materials.
[0104] When the absorber film 4 is a phase shift film formed on the multilayer reflective film 2, the phase difference between the EUV light reflected from the multilayer reflective film 2 and the light reflected from a predetermined thin film needs to be 100 degrees or more, preferably 150 degrees or more, more preferably 180 degrees or more, and even more preferably 200 degrees or more. The phase difference between the EUV light reflected from the multilayer reflective film 2 and the light reflected from a predetermined thin film is preferably 300 degrees or less, more preferably 280 degrees or less, and even more preferably 250 degrees or less. When irradiated with EUV light, the reflectance (relative reflectance) from the absorber film 4 relative to the reflectance from the multilayer reflective film 2 is preferably higher than 3%, and more preferably 4% or more. The relative reflectance is preferably 30% or less, more preferably 20% or less, and even more preferably 10% or less.
[0105] Here, the relative reflectance from the absorber film 4 refers to the reflectance of light reflected from the surface of the absorber film 4 relative to the reflectance of light reflected from the multilayer reflective film 2 (including the protective film 3) when irradiated with EUV light. In other words, the relative reflectance (%) of the absorber film 4 is the value obtained by dividing the reflectance of the absorber film 4 by the reflectance of the multilayer reflective film 2 (including the protective film 3) and multiplying this value by 100.
[0106] The thickness of the lower layer 42 of the absorber film 4 is preferably 2 nm or more in order to function as a buffer layer. In addition, the thickness of the lower layer 42 is preferably 55 nm or less, and more preferably 25 nm or less, in order to reduce the so-called shadowing effect.
[0107] The thickness of the upper layer 44 of the absorber film 4 is preferably 5 nm or more in order to function as the absorber film 4. Furthermore, the thickness of the upper layer 44 is preferably 60 nm or less, more preferably 50 nm or less, and even more preferably 40 nm or less in order to reduce the so-called shadowing effect.
[0108] The absorber film 4 including the lower layer 42 and the upper layer 44 can be formed by magnetron sputtering, such as DC sputtering or RF sputtering. Specifically, the lower layer 42 can be formed using sputtering and a sputtering gas containing the elements contained in the lower layer 42. The same applies to the upper layer 44. For example, the absorber film 4 made of a tantalum compound or the like can be formed by reactive sputtering using a target containing tantalum and boron and argon gas to which oxygen or nitrogen has been added.
[0109] The sputtering gas used to form the lower layer 42 and the upper layer 44 preferably contains a rare gas. The rare gas may be one selected from Xe gas, Ar gas, and Kr gas, or a mixed gas of two or more rare gases selected from these rare gases.
[0110] 1 , the reflective mask blank 100 of this embodiment can have an etching mask film 6 on the absorber film 4. As a material for the etching mask film 6, it is preferable to use a material that has a high etching selectivity of the absorber film 4 to the etching mask film 6 (etching rate of the absorber film 4 / etching rate of the etching mask film 6). The etching selectivity of the absorber film 4 to the etching mask film 6 is preferably 1.5 or more, and more preferably 3 or more.
[0111] The reflective mask blank 100 of this embodiment preferably has an etching mask film 6 on the absorber film 4 .
[0112] In the reflective mask blank 100 of this embodiment, when the absorber film 4 is a predetermined thin film, it is preferable to have an etching mask film 6 formed on the predetermined thin film (absorber film 4) in contact with the predetermined thin film (absorber film 4). Furthermore, it is preferable that the crystallinity of the absorber film 4 is higher than that of the etching mask film 6. Specifically, it is preferable that the crystallite size of the absorber film 4 is 2 nm or more larger than that of the etching mask film 6. When the absorber film 4 includes multiple layers, it is preferable that the crystallinity of the upper layer is higher than that of the etching mask film 6. By using a reflective mask blank 100 having such an etching mask film 6, it is possible to prevent the etching mask film 6 from peeling off at an inappropriate time during the process of manufacturing the reflective mask 200.
[0113] Chromium or a chromium compound is preferably used as the material for the etching mask film 6. Examples of chromium compounds include materials containing Cr and at least one element selected from N, O, C, and H. The etching mask film 6 more preferably contains CrN, CrO, CrC, CrON, CrOC, CrCN, and / or CrOCN, and further preferably is a CrO-based film containing chromium and oxygen (a CrO film, a CrON film, a CrOC film, or a CrOCN film).
[0114] Tantalum or a tantalum compound is preferably used as the material of the etching mask film 6. Examples of tantalum compounds include a material containing Ta and at least one element selected from N, O, B, and H. More preferably, the etching mask film 6 contains TaN, TaO, TaON, TaBN, TaBO, or TaBON.
[0115] Silicon or a silicon compound is preferably used as the material for the etching mask film 6. Examples of silicon compounds include a material containing Si and at least one element selected from N, O, C, and H, as well as metal silicon (metal silicide) and metal silicon compound (metal silicide compound) containing a metal in silicon or a silicon compound. Examples of metal silicon compounds include a material containing a metal, Si, and at least one element selected from N, O, C, and H.
[0116] The thickness of the etching mask film 6 is preferably 3 nm or more in order to form a pattern with high precision in the absorber film 4. Moreover, the thickness of the etching mask film 6 is preferably 15 nm or less in order to make the thickness of the resist film 11 thin.
[0117] <Reflective Mask 200> This embodiment is a reflective mask 200 having an absorber pattern 4a obtained by patterning the absorber film 4 of the reflective mask blank 100 described above.
[0118] As shown in FIG. 3E, the reflective mask 200 of this embodiment has an absorber pattern 4 a formed by patterning an absorber film 4 on the multilayer reflective film 2 or on the protective film 3 of the reflective mask blank 100 described above.
[0119] The absorber pattern 4a corresponds to the "patterned thin film" of this embodiment. The absorber pattern 4a, which is a predetermined patterned thin film, includes a lower layer 42 and an upper layer 44 provided on the lower layer 42, as described above. Therefore, the reflective mask 200 of this embodiment includes a patterned lower layer 42 and an upper layer 44 (shown as a lower layer pattern 42a and an upper layer pattern 44a, respectively, in FIG. 3E ). In the reflective mask 200 of this embodiment, the lower layer pattern 42a is made of a material having an amorphous structure or a microcrystalline structure, and the crystallinity of the upper layer pattern 44a is higher than that of the lower layer pattern 42a. This improves the adhesion between the two layers (the lower layer pattern 42a and the upper layer pattern 44a) of the reflective mask 200 of this embodiment. Furthermore, the predetermined thin films (the lower layer pattern 42a and the upper layer pattern 44a) of the reflective mask 200 of this embodiment can have higher durability.
[0120] 3A to 3E are cross-sectional schematic views showing an example of a method for manufacturing the reflective mask 200. The reflective mask blank 100 of the present embodiment described above can be used to manufacture the reflective mask 200 of the present embodiment. An example of the method for manufacturing the reflective mask 200 will be described below.
[0121] First, a reflective mask blank 100 is prepared, which includes a substrate 1, a multilayer reflective film 2, an absorber film 4 having an upper layer 44 and a lower layer 42, and an etching mask film 6. The reflective mask blank 100 may have a protective film 3. Next, a resist film 11 is formed on the etching mask film 6 to obtain a reflective mask blank 100 with the resist film 11 ( FIG. 3A ). A pattern is written on the resist film 11 using an electron beam lithography device, and a development and rinsing process is then performed to form a resist pattern 11a ( FIG. 3B ).
[0122] Next, the etching mask film 6 is dry-etched using the resist pattern 11a as a mask. As a result, the portions of the etching mask film 6 that are not covered by the resist pattern 11a are etched, forming an etching mask pattern 6a (FIG. 3C). The resist pattern 11a is then removed with a resist remover.
[0123] Next, the absorber film 4 is dry-etched using the etching mask pattern 6a as a mask. As a result, the portions of the absorber film 4 (upper layer 44 and lower layer 42) that are not covered by the etching mask pattern 6a are etched, forming the absorber pattern 4a ( FIG. 3D ). At this time, the upper layer 44 and the lower layer 42 can be etched using different etching gases. For example, when etching the lower layer 42, an etching gas that does not damage the protective film 3 can be used. Furthermore, when etching the upper layer 44, the protective film 3 is not damaged because the lower layer 42 covers the protective film 3. To further reduce the possibility of damage to the protective film 3, an etching gas that has a high etching rate for the upper layer 44 can be used.
[0124] As an etching gas for the absorber film 4 (upper layer 44 and lower layer 42), for example, a fluorine-based gas and / or a chlorine-based gas can be used. As the fluorine-based gas, CF 4 , CHF 3 , C 2 F 6 , C 3 F 6 , C 4 F 6 , C 4 F 8 , C.H. 2 F 2 , C.H. 3 F, C 3 F 8 , SF 6 , and F 2 The chlorine-based gas may be Cl 2 , SiCl 4 , CHCl 3 , CCl 4 , and BCl 3 In addition, a fluorine-based gas and / or a chlorine-based gas and O 2 In this case, a mixed gas containing a predetermined ratio of these may be used. These etching gases may further contain an inert gas such as He and / or Ar, if necessary.
[0125] When the upper layer 44 and the lower layer 42 are etched with different etching gases, it is preferable to use the fluorine-based gas as the etching gas for etching the upper layer 44. In this case, it is also preferable to use the chlorine-based gas as the etching gas for etching the lower layer 42. Depending on the material of the protective film 3, it is also possible to use the chlorine-based gas for etching the upper layer 44 and the fluorine-based gas for etching the lower layer 42.
[0126] Next, after the absorber pattern 4a is formed, the etching mask pattern 6a is removed by dry etching. After the etching mask pattern 6a is removed, a wet cleaning process using an acidic or alkaline aqueous solution is performed to obtain the reflective mask 200 of this embodiment (FIG. 3E).
[0127] The reflective mask 200 thus obtained has a structure in which a multilayer reflective film 2, a protective film 3, and an absorber pattern 4a are laminated on a substrate 1.
[0128] The exposed region (reflective region) of the multilayer reflective film 2 covered by the protective film 3 has the function of reflecting EUV light. The region where the multilayer reflective film 2 and the protective film 3 are covered by the absorber pattern 4a has the function of absorbing EUV light. The reflective mask 200 of this embodiment can improve the adhesion between the upper layer pattern 44a and the lower layer pattern 42a included in the absorber pattern 4a, thereby suppressing film peeling of the reflective mask 200. Furthermore, the reflective mask 200 of this embodiment can have higher durability. By using the reflective mask 200 of this embodiment, a reflective region that maintains high reflectivity for EUV light can be obtained, allowing finer patterns to be transferred to a transfer target object in EUV lithography.
[0129] <Method for Manufacturing Semiconductor Device> The method for manufacturing a semiconductor device of this embodiment includes a step of performing a lithography process using an EUV exposure apparatus 50 using a reflective mask 200 formed by forming a pattern on the above-mentioned predetermined thin film (absorber film 4), and transferring the thin film pattern (absorber pattern 4 a) to a transfer target on a semiconductor substrate, thereby forming a transfer pattern. Figure 4 is a schematic diagram showing an example of the EUV exposure apparatus 50.
[0130] A transfer pattern can be formed on a semiconductor substrate 60 (transfer receiving body) by lithography using the reflective mask 200 of this embodiment. This transfer pattern has a shape that is the result of transferring the pattern of the reflective mask 200. By forming a transfer pattern on the semiconductor substrate 60 using the reflective mask 200, a semiconductor device can be manufactured.
[0131] In the reflective mask 200 of this embodiment, the adhesion between the upper layer pattern 44a and the lower layer pattern 42a included in the absorber pattern 4a can be improved, thereby suppressing film peeling of the reflective mask 200. Furthermore, a reflective mask 200 with higher durability can be obtained. Therefore, by using the reflective mask 200 of this embodiment, a reflective region that maintains high reflectivity for EUV light can be obtained, and therefore a reflective mask 200 with high reflectivity for EUV light can be obtained. Therefore, by using the reflective mask 200 of this embodiment, semiconductor devices can be made with higher density and precision.
[0132] A method of transferring a pattern onto a semiconductor substrate 60 with a resist by using EUV light will be described with reference to FIG.
[0133] 4 shows a schematic configuration of an EUV exposure apparatus 50, which is an apparatus for transferring a transfer pattern onto a resist film 11 formed on a semiconductor substrate 60. The EUV exposure apparatus 50 includes an EUV light generation unit 51, an irradiation optical system 56, a reticle stage 58, a projection optical system 57, and a wafer stage 59, which are precisely arranged along the optical path axis of the EUV light. The container of the EUV exposure apparatus 50 is filled with hydrogen gas.
[0134] The EUV light generation unit 51 has a laser light source 52, a tin droplet generation unit 53, a capture unit 54, and a collector 55. When the high-power carbon dioxide laser from the laser light source 52 irradiates the tin droplets emitted from the tin droplet generation unit 53, the tin droplets are converted into plasma, and EUV light is generated. The generated EUV light is collected by the collector 55 and passes through an irradiation optical system 56 to be incident on a reflective mask 200 set on a reticle stage 58. The EUV light generation unit 51 generates EUV light with a wavelength of, for example, 13.53 nm.
[0135] The EUV light reflected by the reflective mask 200 is reduced by the projection optical system 57 to a pattern image light, typically about one-fourth the original size, and projected onto the semiconductor substrate 60 (transferred substrate). As a result, a given circuit pattern is transferred onto a resist film on the semiconductor substrate 60. A resist pattern can be formed on the semiconductor substrate 60 by developing the exposed resist film. An integrated circuit pattern can be formed on the semiconductor substrate 60 by etching the semiconductor substrate 60 using the resist pattern as a mask. A semiconductor device is manufactured through these and other necessary processes.
[0136] Examples will be described below, but the present invention is not limited to these examples.
[0137] In Examples 1 to 11 and Comparative Examples 1 and 2, a reflective mask blank 100 was produced in which a multilayer reflective film 2, a protective film 3, an absorber film 4, and an etching mask film 6 were formed on the first main surface of a substrate 1. Thereafter, the reflective mask blanks 100 of Examples 1 to 11 and Comparative Examples 1 and 2 were used to produce reflective masks 200 of Examples 1 to 11 and Comparative Examples 1 and 2. Note that for each of Examples 1 to 11 and Comparative Examples 1 and 2, a plurality of reflective mask blanks 100 and a plurality of reflective masks 200 were produced. Measurement values such as crystallite size, which will be described later, are average values of a plurality of samples (specifically, five samples) for each Example and Comparative Example.
[0138] (Reflective mask blank 100) Table 1 shows the composition of the upper layer 44 of the absorber film 4 of the reflective mask blank 100 of the Examples and Comparative Examples, the sputtering gas used in film formation by sputtering, the film thickness, and the crystalline state. Table 2 shows the composition of the lower layer 42 of the absorber film 4 of the reflective mask blank 100 of the Examples and Comparative Examples, the sputtering gas used in film formation by sputtering, the film thickness, and the crystalline state. In the crystalline states shown in Tables 1 and 2, C means a crystalline structure, MC means a microcrystalline structure, and A means an amorphous structure. The absorber films 4 of the Examples and Comparative Examples are all phase shift films having a phase shift function. The reflective mask blanks 100 of the Examples and Comparative Examples were produced as follows.
[0139] A SiO 6025 size (approximately 152 mm x 152 mm x 6.35 mm) low thermal expansion glass substrate 1 with both the first and second main surfaces polished. 2 -TiO 2 A glass substrate 1 was prepared as the substrate 1. To obtain a flat and smooth main surface, polishing was carried out through a rough polishing process, a precision polishing process, a local polishing process, and a touch polishing process.
[0140] Next, a multilayer reflective film 2 was formed on the main surface (first main surface) of the substrate 1. The multilayer reflective film 2 formed on the substrate 1 was a periodic multilayer reflective film made of molybdenum (Mo) and silicon (Si) to be suitable for EUV light with a wavelength of 13.5 nm. The multilayer reflective film 2 was formed by alternately stacking Mo layers and Si layers on the substrate 1 by ion beam sputtering in a krypton (Kr) gas atmosphere using a Mo target and a Si target. First, a Si film was formed to a thickness of 4.2 nm, followed by a Mo film to a thickness of 2.8 nm. This constitutes one cycle, and 40 cycles were similarly stacked. Finally, a Si film was formed to a thickness of 4.0 nm to form the multilayer reflective film 2.
[0141] Next, a protective film 3 made of a RuRhCr film was formed on the multilayer reflective film 2. The protective film 3 was formed to a thickness of 3.5 nm by DC magnetron sputtering using a RuRhCr target (Ru:Rh:Cr=60 at %:30 at %:10 at %) in an Ar gas atmosphere.
[0142] Next, a predetermined absorber film 4 was formed on the protective film 3. The films were formed in the order of a lower layer 42 and an upper layer 44. Only in Comparative Example 1, a top layer was further formed on the upper layer 44.
[0143] As shown in Tables 1 and 2, the absorber membranes 4 of Examples 1 to 11 and Comparative Examples 1 and 2 have a lower layer 42 and an upper layer 44 .
[0144] The lower layer 42 of Examples 1 to 11 and Comparative Example 1 was formed as follows: Table 2 shows the composition of the lower layer 42 of Examples 1 to 11 and Comparative Examples 1 and 2.
[0145] A chromium nitride film (CrN film) was deposited to a thickness of 50 nm on the multilayer reflective film 2 as the lower layer 42 in Examples 1 to 11 and Comparative Example 1. This chromium nitride film was formed by DC magnetron sputtering using a Cr target and a gas in which 10% nitrogen was added to Ar as the sputtering gas.
[0146] The lower layer 42 of Comparative Example 2 was formed as follows.
[0147] A RuZr film was formed as the lower layer 42 of Comparative Example 2. The lower layer 42 of Comparative Example 2 was formed under the following conditions: Target: Ru target and Zr target Sputtering gas: Ar gas Output: 150 W (Ru target), 50 W (Zr target) Film thickness: 5 nm
[0148] Next, the upper layer 44 was formed on the lower layer 42 of Examples 1 to 11 and Comparative Examples 1 and 2. The upper layer 44 was formed as follows. Table 1 shows the compositions of the upper layer 44 of Examples 1 to 11 and Comparative Examples 1 and 2.
[0149] The PtRu film in Example 1 was formed by DC magnetron sputtering using a target containing Pt and Ru and xenon (Xe) as the sputtering gas. Table 1 shows the composition and film thickness of the obtained PtRu film.
[0150] The PtRu film of Example 2 was formed by DC magnetron sputtering using a target containing Pt and Ru and argon (Ar) as the sputtering gas. Table 1 shows the composition and film thickness of the obtained PtRu film.
[0151] The PtRuN film of Example 3 was formed by DC magnetron sputtering (reactive sputtering) using a target containing Pt and Ru and a sputtering gas containing xenon and nitrogen.
[0152] The PtRuN film of Example 4 was formed by DC magnetron sputtering (reactive sputtering) using a target containing Pt and Ru and a sputtering gas consisting of argon and nitrogen. Table 1 shows the composition and thickness of the obtained PtRuN film.
[0153] The PtRuO film of Example 5 was formed by DC magnetron sputtering (reactive sputtering) using a target containing Pt and Ru and a sputtering gas consisting of argon and oxygen. Table 1 shows the composition and film thickness of the obtained PtRuO film.
[0154] The PtRuBN film of Example 6 was formed by DC magnetron sputtering (reactive sputtering) using a target containing Pt, Ru, and B and a sputtering gas consisting of xenon and nitrogen. Table 1 shows the composition and film thickness of the obtained PtRuBN film.
[0155] The PtRuB film of Example 7 was formed by DC magnetron sputtering using a target containing Pt, Ru, and B and xenon (Xe) as the sputtering gas. Table 1 shows the composition and film thickness of the resulting PtRuB film.
[0156] The RuN film of Example 8 was formed by DC magnetron sputtering (reactive sputtering) using a Ru target and a sputtering gas consisting of xenon (Xe) and nitrogen. Table 1 shows the composition and thickness of the obtained RuN film.
[0157] The PtTa film of Example 9 was formed by DC magnetron sputtering (reactive sputtering) using a target containing Pt and Ta and a sputtering gas consisting of xenon (Xe). Table 1 shows the composition and film thickness of the obtained PtTa film.
[0158] The PtRuB film of Example 10 was formed by DC magnetron sputtering using a target containing Pt, Ru, and B and xenon (Xe) as the sputtering gas. Table 1 shows the composition and film thickness of the resulting PtRuB film.
[0159] The PtRuO film of Example 11 was formed by DC magnetron sputtering (reactive sputtering) using a target containing Pt and Ru and a sputtering gas consisting of argon and oxygen. Table 1 shows the composition and film thickness of the obtained PtRuO film.
[0160] The TaBN film (upper layer 44) and the TaBO film (top layer) of Comparative Example 1 were formed as follows.
[0161] A tantalum boron alloy nitride (TaBN) film was formed to a thickness of 50 nm as the upper layer 44 on the lower layer 42 of Comparative Example 1. This TaBN film was formed by DC magnetron sputtering using a target containing Ta and B and Ar with 10% nitrogen added. As shown in Table 1, the composition ratio of this TaBN film was Ta: 0.8, B: 0.1, and N: 0.1. The crystalline state of the TaBN film was amorphous.
[0162] A tantalum boron alloy oxide (TaBO) film was further formed to a thickness of 12 nm as a top layer on the upper layer 44 of Comparative Example 1. This TaBO film was formed by DC magnetron sputtering using a target containing Ta and B and Ar with 30% oxygen added. Between the formation of the upper layer 44 and the formation of the top layer, the DC power was temporarily stopped and the gas used for film formation was changed. The composition ratio of the TaBO film formed here as the top layer was Ta 0.4, B 0.1, and O 0.5. The crystalline state of the TaBO film as the top layer was amorphous.
[0163] The RuN film (upper layer 44) of Comparative Example 2 was formed as follows.
[0164] The RuN film (upper layer 44) of Comparative Example 2 was formed by reactive sputtering using a Ru target and a nitrogen-containing sputtering gas shown in Table 1. Table 1 shows the composition and film thickness of the obtained RuN film. The gas pressure during sputtering was 2.0×10 -1 Pa, and the input power density per target area is 1.7 W / cm 2 The film formation rate was 0.017 nm / sec.
[0165] Next, an etching mask film 6 made of CrN was formed on the absorber film 4 of Examples 1 to 11 and Comparative Examples 1 and 2. The CrN film, which is the etching mask film 6, was formed by DC magnetron sputtering (reactive sputtering) using a target containing Cr and a sputtering gas in which 10% nitrogen was added to Ar. The composition of the CrN film was Cr:N=90 at%:10 at%, and the film thickness was 16 nm.
[0166] In this manner, the reflective mask blanks 100 of Examples 1 to 11 and Comparative Examples 1 and 2 were manufactured.
[0167] (Crystallite Size) The lower layer 42 and the upper layer 44 were formed under the same conditions as those for the absorber film 4 (lower layer 42 and upper layer 44) of the reflective mask blank 100 of Examples 1 to 11 and Comparative Examples 1 and 2, and the crystallite size was measured. An X-ray diffraction profile was obtained using in-plane measurement (2θχ / φ scan) as the X-ray diffraction (XRD) method for a predetermined layer. The crystallite size D was calculated from the diffraction angle u and half-width β of the obtained X-ray diffraction profile using the Scherrer formula (see Formula 2 below). The half-width β was calculated by using the Gaussian function (Formula 1) described above to perform least-squares fitting on the region containing the peak with the highest peak intensity at diffraction angles of 30 degrees to 90 degrees in the X-ray diffraction profile to obtain σ, and substituting this σ into the above-mentioned Formula (3). D = Kλ / β·cos(2 / u) (Formula 2)
[0168] In formula 1, D is the crystallite size (nm), K is the Scherrer constant 0.9, and λ is the X-ray (CuKα 1) is the wavelength of 0.15405 (nm), β is the half width (rad) of the diffraction line width. The diffraction angle u is a value obtained by the fitting.
[0169] The crystallite size of the lower layer 42 determined as described above was less than 1 nm in all of Examples 1 to 11 and Comparative Example 1. The crystallite size of the lower layer 42 in Comparative Example 2 was 7.5 nm.
[0170] The crystallite sizes of the upper layer 44 determined as described above were as follows: The crystallite size of the upper layer 44 in Example 1 was 13.2 nm. The crystallite size of the upper layer 44 in Example 2 was 12.0 nm. The crystallite size of the upper layer 44 in Example 3 was 10.6 nm. The crystallite size of the upper layer 44 in Example 4 was 8.2 nm. The crystallite size of the upper layer 44 in Example 5 was 11.8 nm. The crystallite size of the upper layer 44 in Example 6 was 9.3 nm. The crystallite size of the upper layer 44 in Example 7 was 8.4 nm. The crystallite size of the upper layer 44 in Example 8 was 18 nm. The crystallite size of the upper layer 44 in Example 9 was 15.8 nm. The crystallite size of the upper layer 44 in Example 10 was 4.7 nm. The crystallite size of the upper layer 44 in Example 11 was 3.2 nm. The crystallite size of the upper layer 44 in Comparative Example 1 was less than 1 nm. The crystallite size of the upper layer 44 in Comparative Example 2 was 6.5 nm. In Examples 1 to 11, the difference between the crystallite size of the upper layer 44 and the crystallite size of the lower layer 42 was 2 nm or more. On the other hand, the difference between the crystallite size of the upper layer 44 and the crystallite size of the lower layer 42 in Comparative Examples 1 and 2 was 1 nm or less.
[0171] (Film Density) The upper layer 44 was formed under the same conditions as the upper layer 44 of the absorber film 4 of the reflective mask blank 100 of Examples 1 to 4, and the film densities of the upper layer 44 of Examples 1 to 4 were calculated. The film density was obtained by fitting the X-ray reflectivity obtained by X-ray reflectometry (XRR) to the X-ray reflectivity profile calculated from a thin film model. The film densities of Examples 1 to 4 obtained in this manner were as follows. That is, the film density of the upper layer 44 of Example 1 was 16.4 g / cm 3 The film density of the upper layer 44 in Example 2 was 17.2 g / cm 3 The film density of the upper layer 44 in Example 3 was 11.7 g / cm3 The film density of the upper layer 44 in Example 4 was 17.1 g / cm 3 It was.
[0172] In addition, from the above-mentioned measurement results of crystallite size and film density, it can be seen that when comparing the upper layer of Example 2 and the upper layer of Example 4, the film density is about the same, but the crystallite size is significantly different. Furthermore, when comparing the upper layer of Example 3 and the upper layer of Example 4, the crystallite size of Example 4, which has a higher film density, is smaller. In other words, the upper layer of Example 4, which has a higher film density, has lower crystallinity than the upper layer of Example 3. Therefore, it is considered that the correlation between crystallite size (crystallinity) and film density is low. Furthermore, the upper layer of Example 3 and the upper layer of Example 4 have the same composition ratio, but the film density and crystallite size are not the same. Therefore, it is considered that the correlation between the composition ratio of the film and the crystallite size (crystallinity) or film density is also low.
[0173] (Lattice Plane Spacing of Upper Layer 44) An upper layer 44 was formed under the same conditions as the upper layer 44 of the absorber film 4 of the 100 m reflective mask blanks of Examples 1 to 11, and the lattice plane spacing of the upper layer 44 of Examples 1 to 11 and Comparative Examples 1 and 2 was measured. The upper layer 44 was measured by X-ray diffraction (XRD), and the lattice plane spacing was determined by Bragg's law from the diffraction angle of the X-ray diffraction profile from the upper layer 44 obtained by the measurement. The lattice plane spacing of the upper layer 44 of Examples 1 to 11 was all 0.23 nm or less. As described above, the lattice planes can be those having Miller indices corresponding to the peak with the greatest peak intensity or the peak with the largest peak area within the diffraction angle range of 30 degrees to 90 degrees in the X-ray diffraction profile. In Examples 1 to 11, the lattice plane spacing was determined using the peak with the greatest peak intensity.
[0174] (Reflective mask 200) Next, reflective masks 200 were manufactured using the reflective mask blanks 100 of Examples 1 to 11 and Comparative Examples 1 and 2. The manufacture of the reflective mask 200 will be described with reference to Figures 3A to 3E. Five reflective mask blanks 100 were manufactured for each of the Examples and Comparative Examples.
[0175] First, as shown in FIG. 3A, a resist film 11 was formed on the absorber film 4 of the reflective mask blank 100. A desired pattern, such as a circuit pattern, was then drawn (exposed) on the resist film 11, followed by development and rinsing to form a predetermined resist pattern 11a (FIG. 3B). Next, using the resist pattern 11a as a mask, the etching mask film 6 (CrN film) was dry-etched to form an etching mask pattern 6a (FIG. 3C). Next, the resist pattern 11a was stripped by oxygen ashing. Next, using the resist pattern 11a as a mask, the upper layer 44 of the absorber film 4 was dry-etched, and the lower layer 42 was dry-etched to form an absorber pattern 4a (FIG. 3D). The etching mask pattern 6a was then removed by dry etching (FIG. 3E).
[0176] Finally, wet cleaning was performed using deionized water (DIW), and the reflective masks 200 of Examples 1 to 11 and Comparative Examples 1 and 2 were manufactured.
[0177] (Phase Difference of Phase Shift) The absorber pattern 4a of the reflective masks 200 of Examples 1 to 11 and Comparative Examples 1 and 2 is a pattern of a phase shift film. Therefore, the phase difference between the light reflected from the multilayer reflective film 2 and the light reflected from the absorber film 4 for EUV light was measured for the reflective masks 200 of Examples 1 to 11 and Comparative Examples 1 and 2. The phase difference of the reflective masks 200 of Examples 1 to 11 and Comparative Examples 1 and 2 was between 100 degrees and 300 degrees, and it can be said that they have an appropriate phase shift function.
[0178] (Reflectance of Multilayer Reflective Film 2) When EUV light was irradiated onto the multilayer reflective film 2 of the reflective masks 200 of Examples 1 to 11 and Comparative Examples 1 and 2, the reflectance from the absorber film 4 relative to the reflectance from the multilayer reflective film 2 (relative reflectance) was higher than 3% and not more than 30%. Therefore, it can be said that the relative reflectance of the reflective masks 200 of Examples 1 to 11 and Comparative Examples 1 and 2 was within an appropriate range.
[0179] (Evaluation of Adhesion) When five reflective mask blanks 100 and reflective masks 200 of Examples 1 to 11 were manufactured as described above, no film peeling occurred in any of the samples in the process for manufacturing the reflective mask blank 100 or the process for manufacturing the reflective mask 200. On the other hand, when five reflective mask blanks 100 and reflective masks 200 of Comparative Examples 1 and 2 were manufactured as described above, defects due to peeling of the absorber film 4 occurred in some samples in all of the comparative examples. The peeling of the absorber film 4 was identified as being caused by peeling at the interface between the upper layer 44 and the lower layer 42. Therefore, it can be said that the upper layer 44 and the lower layer 42 of the absorber film 4 of the reflective mask blanks 100 and reflective masks 200 of Examples 1 to 11 of this embodiment have high adhesion.
[0180] (Evaluation of durability) In Examples 1 to 11 and Comparative Examples 1 and 2, a simulation was performed of the exposure transfer image when a defect-free reflective mask 200 was exposed to EUV light and transferred onto a resist film (transfer target) on a semiconductor device. When the exposure transfer image obtained in this simulation was verified, the reflectance and phase shift amount were within the ranges that satisfied the design specifications in all Examples and Comparative Examples. Furthermore, when the reflective masks 200 of Examples 1 to 11 and Comparative Examples 1 and 2 were exposed to EUV light at a cumulative dose of 20 kJ / cm 2 Intermittent irradiation was performed so that the cumulative irradiation amount was 20 kJ / cm 2 corresponds to using the reflective mask 200 approximately 50,000 times. A simulation was carried out of the exposure transfer image when the reflective mask 200 after intermittent irradiation was exposed to and transferred onto a resist film (transfer target) on a semiconductor device using EUV light. When the exposure transfer image obtained by this simulation was examined, it was found that in Examples 1 to 11, the cumulative irradiation dose was 20 kJ / cm 2 The changes in reflectivity and phase shift amount before and after irradiation with EUV light of 100 kJ / cm 2 were within 0.5%. From the above, it can be seen that the reflective mask 200 manufactured from the reflective mask blank 100 of the example of this embodiment has high durability and can be used for exposure transfer with EUV light at a cumulative irradiation dose of, for example, 20 kJ / cm 2. 2On the other hand, in Comparative Example 1, as in the example, the cumulative exposure dose was 20 kJ / cm 2, and the exposure transfer onto the resist film on the semiconductor device was still possible with high accuracy. 2 When the exposed transferred image after irradiation with EUV light of 20 kJ / cm was checked, it was found that some of the reflective masks 200 had a cumulative irradiation dose of 20 kJ / cm 2 The change in reflectance and the change in phase shift amount before and after irradiation with EUV light were greater than 0.5%.
[0181] (Manufacturing of Semiconductor Device) The reflective mask 200 of Examples 1 to 11 was set in an EUV scanner, and EUV exposure was performed on a wafer having a processing film and a resist film formed on a semiconductor substrate 60, which was a transfer object. Then, by developing this exposed resist film, a resist pattern could be formed with high precision on the semiconductor substrate 56 having the processing film formed thereon.
[0182]
[0183]
[0184] REFERENCE SIGNS LIST 1 substrate 2 multilayer reflective film 3 protective film 4 absorber film 4a absorber pattern 5 back surface conductive film 6 etching mask film 6a etching mask pattern 11 resist film 11a resist pattern 42 lower layer 42a lower layer pattern 44 upper layer 44a upper layer pattern 50 EUV exposure apparatus 51 EUV light generation unit 52 laser light source 53 tin droplet generation unit 54 capture unit 55 collector 56 irradiation optical system 57 projection optical system 58 reticle stage 59 wafer stage 60 semiconductor substrate 100 reflective mask blank 200 reflective mask
Claims
1. A reflective mask blank comprising: a substrate; a multilayer reflective film provided on the substrate; and a thin film provided on the multilayer reflective film, the thin film including a lower layer and an upper layer provided on the lower layer, the lower layer being made of a material having an amorphous structure or a microcrystalline structure, and the upper layer having a higher crystallinity than the lower layer.
2. The reflective mask blank according to claim 1, wherein the lower layer and the upper layer are in contact with each other.
3. A reflective mask blank according to claim 1 or 2, characterized in that the thin film is an absorber film.
4. A reflective mask blank according to claim 1 or 2, characterized in that the difference between the crystallite size of the upper layer and the crystallite size of the lower layer is 2 nm or more.
5. A reflective mask blank according to claim 1 or 2, further comprising an etching mask film formed on and in contact with said thin film, said etching mask film having lower crystallinity than said upper layer.
6. The reflective mask blank according to claim 1 or 2, further comprising a protective film between the multilayer reflective film and the thin film.
7. A reflective mask blank according to claim 1 or 2, characterized in that the lower layer and the upper layer are made of different materials.
8. A reflective mask blank according to claim 1 or 2, characterized in that the upper layer contains at least one selected from Ag, Au, Pt, Pd, Ir, Re, Os, Ru, Ta, Cr, Ti, Nb, Mo, W and Rh.
9. A reflective mask blank according to claim 1 or 2, characterized in that the crystallite size of the upper layer is greater than 3 nm.
10. A reflective mask comprising: a substrate; a multilayer reflective film provided on the substrate; and a thin film having a pattern provided on the multilayer reflective film, the thin film including a lower layer and an upper layer provided on the lower layer, the lower layer being made of a material having an amorphous structure or a microcrystalline structure, and the upper layer having a higher crystallinity than the lower layer.
11. The reflective mask according to claim 10, wherein said lower layer and said upper layer are in contact with each other.
12. The reflective mask according to claim 10 or 11, wherein the thin film is an absorber film.
13. The reflective mask according to claim 10, wherein the difference between the crystallite size of the upper layer and the crystallite size of the lower layer is 2 nm or more.
14. The reflective mask according to claim 10 or 11, further comprising a protective film between said multilayer reflective film and said thin film.
15. The reflective mask according to claim 10 or 11, characterized in that the lower layer and the upper layer are made of different materials.
16. The reflective mask according to claim 10 or 11, characterized in that the upper layer contains at least one selected from Ag, Au, Pt, Pd, Ir, Re, Os, Ru, Ta, Cr, Ti, Nb, Mo, W and Rh.
17. The reflective mask according to claim 10 or 11, characterized in that the crystallite size of the upper layer is greater than 3 nm.
18. A method for manufacturing a semiconductor device, comprising the steps of: forming a reflective mask in which a pattern is formed on the thin film of the reflective mask blank described in claim 1; or using the reflective mask described in claim 10 to transfer the pattern to a transfer target on a semiconductor substrate.
Citation Information
Patent Citations
Reflecting mask blank and reflecting type mask and its manufacturing method
JP2004039884A
Reflective mask blank for EUV lithography
JP2015008265A
Reflection type mask blank, reflection type mask, substrate with conductive film, and method for manufacturing semiconductor device
JP2021128247A
Reflection-type mask blank, reflection-type mask and method for manufacturing same, and method for manufacturing semiconductor device
WO2020184473A1
Cited By