Adhesive agent composition, adhesive laminate, and composite member
The adhesive laminate, composed of specific resin and rubber components with imidazole curing agents, addresses the challenges of adhesive thickness and curing time, providing rapid curing and strong bonding for metal-resin integration in automotive applications.
Patent Information
- Application Number
- PCT/JP2024/008653
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-07
- Publication Date
- 2024-10-03
AI Technical Summary
Existing adhesive technologies face challenges in adjusting adhesive coating thickness, separating issues with nonwoven fabrics, and prolonged curing times, which lead to poor bonding strength and stress absorption during the integration of metal and resin materials, particularly in automotive electronic device housings.
An adhesive laminate comprising a thermosetting resin with maleimide and resol type phenolic resins, a thermoplastic resin with acid-modified nitrile rubber, and a curing agent with imidazoles having a high reaction initiation temperature, along with a plasticizer, is used, featuring a short curing time and excellent stress relaxation properties, integrated with a base material layer and adhesive-impregnated layer for improved bonding.
The adhesive laminate achieves rapid curing and enhanced stress relaxation, ensuring strong bonding between metal and resin layers while maintaining process efficiency and storage stability, suitable for automotive and precision parts manufacturing.
Smart Images

Figure JP2024008653_03102024_PF_FP_ABST
Abstract
Description
Adhesive composition, adhesive laminate, and composite member
[0001] The present invention relates to an adhesive composition, an adhesive laminate, and a composite member.
[0002] Molded products (composite members) in which a metal material and a resin (hereinafter sometimes referred to as "molded resin") are integrated are used as housings for in-vehicle electronic devices, etc. Known methods for integrating a metal material and a resin include joining or adhering the surfaces of the metal material and the resin via an adhesive or an adhesive sheet. For example, Patent Document 1 discloses an adhesive containing an epoxy resin, an acrylic resin, and a curing agent, and an adhesive sheet having an adhesive layer in which the adhesive is impregnated into a core material (woven fabric or nonwoven fabric).
[0003] JP 2014-70221 A
[0004] When using an adhesive to integrate metal materials and resins, there is a problem in that it is difficult to adjust the adhesive coating thickness. On the other hand, when using an adhesive sheet in which a core material such as a nonwoven fabric is impregnated with an adhesive, there are strength-related issues, such as the tendency for the nonwoven fabric and the adhesive to peel off, or for the resin to be bonded to the nonwoven fabric to peel off. Furthermore, shortening the adhesive curing time leads to shorter process times and contributes to improved productivity. However, in both cases, there is a problem in that the adhesive curing time is long. When the adhesive curing time is shortened, the adhesive curing reaction becomes rapid, and the dimensional change (cure shrinkage) of the adhesive due to the curing reaction also becomes rapid. Rapid dimensional change in the adhesive cannot fully absorb the stress generated at the interface with the bonded components, resulting in poor bonding. Therefore, shortening the adhesive curing time may result in a decrease in bonding strength. In consideration of the above-mentioned problems, the present invention aims to provide a technology related to an adhesive laminate with a short adhesive curing time and excellent stress relaxation properties.
[0005] One aspect of the present invention is an adhesive composition. The adhesive composition includes a thermosetting resin containing a maleimide resin and a resole-type phenolic resin, a thermoplastic resin containing an acid-modified nitrile rubber, and a curing agent containing an imidazole having a reaction initiation temperature of 70°C or higher. The adhesive composition of the above aspect may include 10 to 400 parts by mass of the resole-type phenolic resin per 100 parts by mass of the maleimide resin. The adhesive composition may include 20 to 400 parts by mass of the acid-modified nitrile rubber per 100 parts by mass of the maleimide resin and the resole-type phenolic resin. The adhesive composition may include 1 to 10 parts by mass of the imidazole per 100 parts by mass of the maleimide resin, the resole-type phenolic resin, and the acid-modified nitrile rubber. The imidazole may be insoluble in methyl ethyl ketone and tetrahydrofuran. The adhesive composition may further include a plasticizer.
[0006] Another aspect of the present invention is an adhesive laminate. The adhesive laminate comprises a base layer containing a woven fabric or a nonwoven fabric, and an adhesive layer laminated on one main surface of the base layer and containing an adhesive composition, wherein an adhesive-impregnated layer impregnated with the adhesive composition is formed in a portion of the base layer adjacent to the adhesive layer, and the adhesive composition is the adhesive composition of any of the above-mentioned aspects. In the adhesive laminate of the above aspect, the woven fabric or the nonwoven fabric may have a melting point of 150°C or higher. The adhesive layer may have a thickness of 5 to 100 μm. The base layer may have a thickness of 5 to 200 μm, and the adhesive-impregnated layer may have a thickness of 1 to 95 μm.
[0007] Yet another aspect of the present invention is a composite member, in which a metal layer and a resin layer are joined via the adhesive laminate of the above-described aspect, the metal layer is in contact with the adhesive layer, and a resin layer containing a resin is in contact with the base layer on the side opposite to the side on which the adhesive layer is laminated, and a resin-impregnated layer impregnated with the resin is formed in a part of the base layer on the side in contact with the resin layer.
[0008] According to the present invention, a technique can be provided for an adhesive laminate in which the curing time of the adhesive is short and which has excellent stress relaxation properties.
[0009] Fig. 1 is a schematic cross-sectional view showing the configuration of an adhesive laminate according to an embodiment. Fig. 2 is a schematic cross-sectional view showing the configuration of a composite member according to an embodiment. Figs. 3(a) to 3(d) are cross-sectional views showing steps in a method for producing a composite member.
[0010] Hereinafter, embodiments of the present invention will be described in detail. In this specification, the notation "a to b" in the description of a numerical range means a to b, unless otherwise specified. Hereinafter, adhesive compositions (sometimes referred to as adhesives) according to embodiments, adhesive laminates using the adhesive compositions, and composite members will be described in order.
[0011] (Adhesive Composition) The adhesive composition according to the embodiment contains a thermosetting resin, a thermoplastic resin, and a curing agent. Each component contained in the adhesive composition will be described in detail below.
[0012] <Thermosetting Resin> The thermosetting resin includes a maleimide resin and a resol-type phenolic resin.
[0013] The maleimide resin preferably has two or more maleimide groups. Specific examples include 4,4'-diphenylmethane bismaleimide, m-phenylene bismaleimide, 4-methyl-1,3-phenylene bismaleimide, bisphenol A diphenyl ether bismaleimide, 4,4'-diphenyl ether bismaleimide, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, and 4,4'-diphenylsulfone bismaleimide.
[0014] Examples of raw materials for resol-type phenolic resins include alkyl-substituted phenols such as phenol, cresol, and p-t-butylphenol, cyclic alkyl-modified phenols such as terpene and dicyclopentadiene, those having functional groups containing heteroatoms such as nitro groups, halogen groups, amino groups, and cyano groups, and those having skeletons such as naphthalene and anthracene. Any of these may be used alone or in combination of two or more.
[0015] The amount of the resol type phenolic resin blended is preferably 10 to 400 parts by mass, more preferably 50 to 300 parts by mass, per 100 parts by mass of the maleimide resin.
[0016] <Thermoplastic Resin> The thermoplastic resin includes acid-modified nitrile rubber. Examples of acid-modified nitrile rubber include maleic acid nitrile rubber and carboxylic acid-modified nitrile rubber (carboxy group-containing acrylonitrile butadiene copolymer). Of these, carboxylic acid-modified nitrile rubber is preferred from the viewpoints of compatibility with thermosetting resins, reaction promotion, solubility in solvents, and application processability. The amount of thermoplastic resin blended is preferably 20 to 400 parts by mass, more preferably 40 to 200 parts by mass, per 100 parts by mass of the combined amount of the maleimide resin and resole-type phenolic resin described above. By setting the blending amount of thermoplastic resin within the above range, the rapid curing property can be improved without impairing the toughness of the resulting adhesive.
[0017] <Curing Agent> The curing agent contains an imidazole (hereinafter sometimes simply referred to as "imidazole") having a reaction initiation temperature of 70°C or higher, preferably 90°C or higher. The imidazoles include 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine (reaction initiation temperature: 116°C), 2',4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine (reaction initiation temperature: 136°C), 2',4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct (reaction initiation temperature: 120°C), 2-phenyl-4'5-dihydroxymethylimidazole (reaction initiation temperature: 146°C), 2-phenyl-4-methyl-5-hydroxymethylimidazole (reaction initiation temperature: 130°C), 2',4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine (reaction initiation temperature: 120°C) and the like.
[0018] By setting the reaction initiation temperature of the imidazole to 70°C or higher, the initiation of the reaction can be suppressed when the adhesive composition is applied and dried. Furthermore, it is preferable that the imidazole is insoluble in methyl ethyl ketone and tetrahydrofuran. This can improve the long life of the adhesive composition.
[0019] The amount of imidazole compounded is preferably 1 to 10 parts by mass, and more preferably 3 to 9 parts by mass, per 100 parts by mass of the total amount of the maleimide resin, resole phenolic resin, and acid-modified nitrile rubber. By setting the amount of imidazole compounded to 1 part by mass or more, rapid curing properties can be improved. Furthermore, by setting the amount of imidazole compounded to 100 parts by mass or less, the usable time of the resulting adhesive after application can be extended.
[0020] <Plasticizer> The adhesive composition according to the embodiment may contain a plasticizer. This can improve the workability (adhesion) when applying the adhesive composition and the stress relaxation properties when the adhesive composition is dried. Examples of plasticizers include acrylic esters, phthalic esters, adipic esters, phosphate esters, trimellitic esters, citric esters, epoxies, and polyesters. Two or more of these plasticizers may be used.
[0021] The amount of plasticizer blended is preferably 1 to 100 parts by mass, and more preferably 5 to 50 parts by mass, per 100 parts by mass of the total amount of the maleimide resin, resol-type phenolic resin, acid-modified nitrile rubber, and imidazoles described above. By blending the amount of plasticizer at 1 part by mass or more, the stress relaxation properties of the resulting adhesive can be further improved. By blending the amount of plasticizer at 100 parts by mass or less, the adhesive can be prevented from becoming too tacky and the fast curing properties can be improved.
[0022] <Other Components> The adhesive composition may contain fillers and additives as other components, such as inorganic fillers, flame retardants, conductivity imparting agents, crystal nucleating agents, ultraviolet absorbers, antioxidants, vibration dampers, antibacterial agents, insect repellents, deodorizing agents, coloration inhibitors, heat stabilizers, antistatic agents, plasticizers, lubricants, colorants, foaming agents, foam control agents, coupling agents, tackifiers and other tackifying resins, and curing agents.
[0023] (Adhesive laminate) Fig. 1 is a schematic cross-sectional view showing the configuration of an adhesive laminate 10 according to an embodiment. As shown in Fig. 1, the adhesive laminate 10 includes an adhesive layer 20 and a base layer 30.
[0024] <Adhesive Layer> The adhesive layer 20 is laminated on one main surface of the base layer 30. The adhesive layer 20 contains the adhesive composition described above.
[0025] The thickness of the adhesive layer 20 is preferably 5 to 100 μm, and more preferably 10 to 50 μm. By setting the lower limit of the thickness of the adhesive layer 20 to the above value, the adhesive strength can be increased. On the other hand, by setting the upper limit of the thickness of the adhesive layer 20 to the above value, it is possible to prevent air bubbles from remaining in the adhesive layer 20, and thus to increase the adhesiveness.
[0026] <Base Material Layer> The base material layer 30 preferably includes a woven fabric or a nonwoven fabric, and more preferably includes a nonwoven fabric. Examples of fibers constituting the woven fabric or nonwoven fabric include engineering plastic fibers such as polyphenylene sulfide (PPS) fibers, polyethylene terephthalate (PET) fibers, polyamide (PA) fibers, and polybutylene terephthalate (PBT) fibers, as well as fibers made of Teflon (registered trademark), glass, carbon, ceramic, metal, etc.
[0027] The air permeability of the base layer 30 is 1 to 150 cc / (cm 2 · seconds), and 15 to 150 cc / (cm 2 10 seconds) is more preferable. By setting the lower limit of the air permeability of the base material layer 30 to the above value, when a molded resin (resin layer) and a metal layer are bonded via the adhesive laminate 10, a part of the molded resin can be easily penetrated into the base material layer 30, thereby increasing the bonding strength. By setting the upper limit of the air permeability of the base material layer 30 to the above value, the strength of the base material layer 30 can be made sufficient.
[0028] The melting point of the base material layer 30 is preferably 150° C. or higher, and more preferably 200° C. or higher. By setting the lower limit of the melting point of the base material layer 30 to the above value, it is possible to ensure the heat resistance required to maintain the shape during thermocompression molding.
[0029] The tensile strength of the base material layer 30 is preferably 0.05 to 8.0 kN / m, and more preferably 0.2 to 6.0 kN / m. By setting the lower limit of the tensile strength of the base material layer 30 to the above value, it is possible to prevent the base material layer 30 from breaking, and thus to increase the bonding strength. By setting the upper limit of the tensile strength of the base material layer 30 to the above value, it is possible to increase the bonding strength. Note that the tensile strength and porosity of the base material layer 30 are negatively correlated. Therefore, it is presumed that by setting the upper limit of the tensile strength of the base material layer 30 to the above value, the porosity of the base material layer 30 does not become too low, making it easier for the resin to sufficiently penetrate into the base material layer 30, thereby increasing the bonding strength.
[0030] An adhesive-impregnated layer 32 impregnated with an adhesive composition is formed on a portion of the base material layer 30 adjacent to the adhesive layer 20 .
[0031] The thickness of the base layer 30 is preferably 5 to 200 μm, more preferably 10 to 100 μm. By setting the lower limit of the thickness of the base layer 30 to the above value, sufficient room for a portion of the molding resin to penetrate into the base layer 30 can be provided, thereby increasing adhesive strength. Setting the upper limit of the thickness of the base layer 30 to the above value can prevent damage to portions of the base layer 30 that are not impregnated with adhesive or molding resin after laminate molding due to load. Furthermore, by leaving a fiber layer that is not impregnated with either adhesive or molding resin in the base layer 30 after laminate molding, stress resulting from dimensional changes in each component can be absorbed, preventing delamination during molding. The thickness of the adhesive-impregnated layer 32 of the base layer 30 is preferably 1 to 95 μm, more preferably 5 to 50 μm. Setting the lower limit of the thickness of the adhesive-impregnated layer 32 to the above value can prevent delamination between the adhesive layer 20 and the base layer 30 during laminate molding with the molding resin. On the other hand, by setting the upper limit of the thickness of the adhesive-impregnated layer 32 to the above value, the thickness of the portion not impregnated with adhesive (the portion containing only the base layer 30) can be ensured to be sufficient, thereby enabling the anchoring effect between the molding resin and the base layer 30 to be fully achieved. Furthermore, the adhesive can be prevented from seeping out from the surface of the base layer 30 opposite the adhesive layer 20. The thickness of the portion of the base layer 30 not impregnated with adhesive (the region designated by reference numeral 34 in FIG. 1 ) is preferably 1 to 199 μm, more preferably 5 to 95 μm. By setting the lower limit of the thickness of the portion not impregnated with adhesive (the portion containing only the base layer 30) to the above value, the anchoring effect between the molding resin and the base layer 30 can be fully achieved, thereby preventing peeling between the molding resin and the base layer 30. On the other hand, by setting the upper limit of the thickness of the portion not impregnated with adhesive (the portion containing only the base layer 30) to the above value, the portion of the base layer 30 not impregnated with adhesive or molding resin after laminate molding can be prevented from being destroyed by load, thereby increasing the adhesive strength.
[0032] In addition to the effects described above, the adhesive laminate 10 described above exhibits at least the following effects: The adhesive has a short curing time and excellent stress relaxation properties. Since the adhesive is held in the base layer 30, not only is the adhesive prevented from flowing at high temperatures, but after molding, the base layer 30 absorbs thermal stress caused by slow cooling, thereby preventing peeling after molding. Since resin molding is possible while the adhesive laminate is attached to the metal material, it is easy to incorporate into composite material manufacturing processes (e.g., BMC molding, SMC molding, RTM molding, VaRTM molding, autoclave molding, etc.), and the process of integrating the metal material and the molded resin can be easily and efficiently performed. Since the adhesive laminate 10 according to the embodiment is in the form of a sheet that is solid at room temperature, compared to solvent-containing liquid adhesives, there is no concern about changes in solid content or increases in paint viscosity due to solvent evaporation during storage, and therefore it has excellent storage stability.
[0033] (Method of Manufacturing Adhesive Laminate) In a method of manufacturing the adhesive laminate 10 according to the embodiment, a predetermined amount of solvent-containing adhesive composition is applied to a release film such as PET, and the solvent is removed using a ventilated oven or the like to produce a sheet with an adhesive layer. A base layer 30 is laminated on the obtained sheet with a pressure-sensitive adhesive layer (adhesive layer with release film), and a temperature of 80 to 200°C is applied to impregnate a portion of the base layer 30 with the molten adhesive. This forms an adhesive-impregnated layer 32 of a predetermined thickness on a portion of the base layer 30. The thickness of the adhesive-impregnated layer 32 can be adjusted to a desired value by adjusting the amount of adhesive applied, the temperature applied, and the pressure applied during lamination.
[0034] Examples of the solvent used include organic solvents such as hydrocarbons, alcohols, ketones, and ethers, as well as water. Specific examples of the organic solvent include acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, cyclopentanone, toluene, xylene, ethyl acetate, butyl acetate, tetrahydrofuran, N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, dimethyl sulfoxide, ethylene glycol monomethyl ether acetate, propylene glycol dimethyl ether, benzenedioxane, cyclopentyl methyl ether, methylene chloride, chloroform, 1,2-dichloroethane, γ-butyrolactone, cellosolve, butyl cellosolve, carbitol, and butyl carbitol. In particular, from the viewpoint of storage stability, solvents having a boiling point lower than the activation temperature (reaction initiation temperature) of the curing agent are preferred, and acetone, methyl ethyl ketone, toluene, ethyl acetate, and tetrahydrofuran are particularly desirable. The above-mentioned solvents may be used alone or in combination of two or more. The solvent is preferably one that dissolves the above-mentioned thermosetting resin and thermoplastic resin, and is also preferably one that does not dissolve imidazoles and can disperse them uniformly.
[0035] (Composite member) Figure 2 is a schematic cross-sectional view showing the configuration of a composite member 100 according to an embodiment. The composite member 100 according to an embodiment has a structure in which a metal layer 110 and a resin layer 120 are bonded via the adhesive laminate 10 described above. The metal layer 110 is in contact with the adhesive layer 20 described above, and the metal layer 110 and the resin layer 120 are bonded via the adhesive laminate 10 so that the resin layer 120 containing a resin is in contact with the base layer 30 on the side opposite to the side on which the adhesive layer 20 is laminated. A resin-impregnated layer 36 impregnated with resin is formed in a portion of the base layer 30 on the side in contact with the resin layer 120. Applications of the composite member 100 include composite members for use in automobiles and precision parts.
[0036] (Method of manufacturing a composite member) FIGS. 3( a) to 3(d) are cross-sectional views illustrating steps in a method of manufacturing a composite member. As shown in FIG. 3(a), a metal layer 110 is set in a mold (not shown). Examples of materials for the metal layer 110 include SUS, aluminum, copper, and plated (e.g., Ni-plated or Sn-plated) metal materials. Meanwhile, an adhesive laminate 10 is prepared in which a release film 40 is laminated on an adhesive layer 20. Examples of materials for the release film 40 include PET (polystyrene terephthalate). Next, as shown in FIG. 3(b), the release film 40 is peeled off, and the adhesive laminate 10 is attached to the metal layer 110. When a thermosetting resin is used as the adhesive for the adhesive layer 20, by attaching the adhesive laminate 10 to the metal layer 110 and then heating to harden the adhesive, the metal layer 110 and the adhesive layer 20 are firmly adhered to each other and heat resistance can be imparted. Next, as shown in FIG. 3( c), a molded resin 122 is laminated by heating and pressurizing onto the main surface of the adhesive laminate 10 opposite the surface to which the metal layer 110 is attached. At this time, a portion of the molten molded resin 122 flows into the base layer 30, along with the molten adhesive. This creates an anchor effect between the molded resin 122 and the base layer 30, firmly bonding the metal layer 110 and the molded resin 122. Examples of the molded resin 122 include engineering plastics or super engineering plastics such as PPS, PBT, and PA. Next, as shown in FIG. 3( d), after the laminate is completed, the mold is demolded. This allows a portion of the molded resin 122 (see FIG. 3( c)) to impregnate a portion of the base layer 30, forming a resin-impregnated layer 36, thereby obtaining a composite member 100 in which the resin layer 120 and the metal layer 110 are bonded via the adhesive laminate 10. The molding conditions vary depending on the type of molding resin 122, but for example, molding resin 122 can be molded under conditions such as a press temperature of 150° C., a press pressure of 0.1 MPa, and a holding time of 5 minutes.
[0037] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various other configurations can also be adopted.
[0038] EXAMPLES The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to these.
[0039] (Preparation of adhesive sheet) Test pieces of adhesive sheets were prepared using the following procedure. <Preparation of adhesive sheet with release film> An adhesive sheet with a release film was prepared using the following procedure. - An adhesive composition with the components and amounts shown in Table 1 was applied to a release film (a PET film that had been subjected to a release treatment). - Heating was carried out in a ventilated oven at 60°C for 5 minutes (at a temperature below the reaction initiation temperature of the curing agent contained in the resin composition) to remove the solvent from the resin composition. - The sheet was removed from the ventilated oven to obtain an adhesive sheet with a release film having an adhesive sheet with a thickness of 20 μm.
[0040] (Curing of Adhesive Composition) The resulting adhesive sheet with release film was heated in a ventilated oven (heating conditions: 150°C / 5 minutes). The sheet was then removed from the ventilated oven, and adhesive sheet A that had been subjected to a heat treatment was obtained.
[0041] (Rapid curing property) The adhesive layer of adhesive sheet A was removed from the PET film to obtain a test piece (size: 8 mm x 10 mm). Using this test piece, the tensile storage modulus was measured using a DMA (Dynamic Mechanical Analyzer) device (Vibron measuring instrument, manufactured by Hitachi High-Tech Science Corporation, DMS6100). The storage modulus measurement was performed under conditions of a frequency of 10 Hz, a heating rate of 5°C / min, and a load of 10 mN. The storage modulus was measured at 80°C. Based on the obtained storage modulus, the fast curing property was evaluated according to the following fast curing property evaluation criteria. The evaluation results of fast curing property are shown in Table 1. <Rapid curing property evaluation criteria> A: 1 MPa or more B: 0.1 MPa or more but less than 1 MPa C: Less than 0.1 MPa
[0042] (Stress Relaxation) The adhesive sheet A and a nonwoven fabric (PET fiber) were heat-laminated using a roll laminator to obtain an adhesive sheet with nonwoven fabric tape. The lamination conditions were a temperature of 80°C, a pressure of 4 N / cm, and a pressing speed of 1 m / min. The obtained adhesive sheet with nonwoven fabric tape was cut to a size of φ25 mm and attached to a 50 mm square aluminum sheet A5052. A φ25 mm sealing resin (epoxy molding resin (EME-G631BQ) manufactured by Sumitomo Bakelite Co., Ltd.) was laminated on the top surface of the adhesive sheet with nonwoven fabric tape at a press temperature of 150°C, a holding time of 5 minutes, and a press pressure of 0.1 MPa to obtain a laminated sample. The obtained laminated sample was cooled to room temperature and the presence or absence of bonding was confirmed. Based on the presence or absence of bonding, stress relaxation was evaluated according to the following stress relaxation evaluation criteria. The stress relaxation evaluation results are shown in Table 1. <Stress Relaxation Evaluation Criteria> A: Bonded C: Unbonded
[0043] (Adhesion) Adhesion was evaluated as follows. The above-mentioned adhesive sheet was cut into a size of 5 mm x 5 mm and attached to an aluminum material (A5052 material). A sealing resin was laminated on the upper surface of the adhesive sheet at a press temperature of 150°C, a holding time of 5 minutes, and a press pressure of 0.1 MPa to obtain a shear strength measurement sample. Epoxy molding resin (EME-G631BQ) manufactured by Sumitomo Bakelite Co., Ltd. was used as the sealing resin. The shear strength of the shear strength measurement sample was measured using a digital loading device SL-5000 manufactured by Imada Manufacturing Co., Ltd. at a shear rate of 50 mm / min and 80°C. Based on the obtained shear strength, adhesion was evaluated according to the following adhesion evaluation criteria. The evaluation results of adhesion are shown in Table 1. <Adhesion Evaluation Criteria> A: 1 MPa or more B: 0.1 MPa or more but less than 1 MPa C: Less than 0.1 MPa
[0044] (Overall Evaluation) Based on the three evaluation items described above, an overall evaluation was made using the following criteria. A: All three evaluation items were judged as "A". B: Of the three evaluation items, one or more items were judged as "B", and the remaining evaluation items were all judged as "A". C: Of the three evaluation items, one or more items were judged as "C".
[0045]
[0046] REFERENCE SIGNS LIST 10 adhesive laminate, 20 adhesive layer, 30 substrate layer, 32 adhesive-impregnated layer, 34 portion not impregnated with adhesive, 36 resin-impregnated layer, 100 composite member, 110 metal layer, 120 resin layer, 122 molded resin
Claims
1. An adhesive composition comprising: a thermosetting resin containing a maleimide resin and a resol-type phenolic resin; a thermoplastic resin containing an acid-modified nitrile rubber; and a curing agent containing an imidazole having a reaction initiation temperature of 70°C or higher.
2. The adhesive composition according to claim 1, comprising 10 to 400 parts by mass of the resol type phenolic resin per 100 parts by mass of the maleimide resin.
3. The adhesive composition according to claim 1, comprising 20 to 400 parts by mass of an acid-modified nitrile rubber per 100 parts by mass of the total amount of the maleimide resin and the resol type phenolic resin.
4. The adhesive composition according to claim 1, comprising 1 to 10 parts by mass of the imidazoles per 100 parts by mass of the total amount of the maleimide resin, the resol type phenolic resin, and the acid-modified nitrile rubber.
5. The adhesive composition of claim 1, wherein said imidazoles are insoluble in methyl ethyl ketone and tetrahydrofuran.
6. The adhesive composition of claim 1, further comprising a plasticizer.
7. An adhesive laminate comprising: a base layer containing a woven fabric or a nonwoven fabric; and an adhesive layer containing an adhesive composition laminated on one main surface of the base layer, wherein an adhesive-impregnated layer is formed in which the adhesive composition is impregnated in a part of the base layer on the side adjacent to the adhesive layer, and the adhesive composition is an adhesive composition according to any one of claims 1 to 6.
8. The adhesive laminate according to claim 7, wherein the melting point of said woven fabric or said nonwoven fabric is 150° C. or higher.
9. The adhesive laminate according to claim 7, wherein the adhesive layer has a thickness of 5 to 100 μm.
10. The adhesive laminate according to claim 7, wherein the thickness of said base layer is 5 to 200 μm, and the thickness of said adhesive-impregnated layer is 1 to 95 μm.
11. A composite member in which a metal layer and a resin layer are bonded via the adhesive laminate described in claim 7, the metal layer is in contact with the adhesive layer, and the resin layer containing a resin is in contact with the base layer on the side opposite to the side on which the adhesive layer is laminated, and a resin-impregnated layer in which the resin is impregnated is formed in a portion of the base layer on the side in contact with the resin layer.
Citation Information
Patent Citations
High temperature resistant halogen-free flame-retardant adhesive for flexible copper clad foil substrate and preparation thereof
CN101323773A
High temperature resistant halogen-free antiflaming adhesive for flexible printed circuit board
CN103834342A
Liquid adhesive for electronic parts and adhesive tape
WO2011118664A1