Method for manufacturing cutting tool, and cutting tool

The ultraviolet laser peening method for cutting tools addresses the peeling and wear resistance issues of conventional hard-coated cutting tools by applying compressive residual stress directly to the tool base, enhancing fracture and wear resistance and simplifying the manufacturing process.

WO2024203106A1PCT designated stage expired Publication Date: 2024-10-03MITSUBISHI MATERIALS CORP

Patent Information

Application Number
PCT/JP2024/008697
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-07
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional cutting tools with hard coatings face issues of peeling and reduced wear resistance due to tensile residual stress and peeling of oxide layers, especially when subjected to laser peening, which complicates the manufacturing process and increases costs.

Method used

The method involves forming a hard coating with an oxide layer on a sintered alloy tool base and using an ultraviolet laser peening process with a wavelength of 190 nm to 380 nm and pulse widths of 30 fs to 2 ps, directly irradiating the tool base to apply compressive residual stress without peeling the oxide layer, thereby enhancing fracture and wear resistance.

Benefits of technology

This approach stabilizes the application of high compressive residual stress to the tool base surface, improving wear resistance and chipping resistance while simplifying the manufacturing process and reducing costs, allowing for a broader range of cutting conditions and tool applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024008697_03102024_PF_FP_ABST
    Figure JP2024008697_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This method for manufacturing a cutting tool (10) comprises: a film formation step (S2) for forming a hard coating film (2) that has an oxide layer (22), at least, on the surface of a tool base body (1) that is formed of a sintered alloy; and an ultraviolet laser peening step (S3) for directly irradiating the hard coating film (2) with a pulse laser having, in a gas, a wavelength of 190 nm to 380 nm (inclusive) and a pulse width of 30 fs to 2 ps (inclusive). Due to the ultraviolet laser peening step (S3), a compressive residual stress is imparted to a surface layer (1a) of the tool base body (1) immediately below the oxide layer (22), while leaving the oxide layer (22) in the hard coating film (2).
Need to check novelty before this filing date? Find Prior Art

Description

Cutting tool manufacturing method and cutting tool

[0001] This application claims priority to Japanese Patent Application No. 2023-051135, filed on March 28, 2023, the contents of which are incorporated herein by reference.

[0002] Conventionally, cutting tools have been known in which a hard coating is formed on a tool substrate made of cemented carbide. In these types of hard-coated cutting tools, shot peening or laser peening is performed after the hard coating is formed, imparting compressive residual stress to the surface layer of the tool substrate and the hard coating, thereby improving the chipping resistance of the cutting edge. It is also generally known that laser peening can produce higher compressive residual stress than shot peening. However, a problem with laser peening is that it easily damages the surface of the hard coating.

[0003] The methods for forming hard coatings used on cutting tools are roughly divided into chemical vapor deposition (CVD) and physical vapor deposition (PVD). Of these, the hard coatings formed by CVD, which tend to leave residual tensile stress after film formation, are the ones that pose a challenge to chipping resistance at the cutting edge. A typical hard coating for cutting tools formed by CVD is composed of, in order from the tool substrate side, TiCN, Al, 2 O 3 In order to add aesthetic appeal to the exterior design, a TiN film is formed as the outermost layer with a thickness of about 1 μm. In laser peening, the AlN oxide layer is particularly 2 O 3 The problem is that the layers tend to peel off easily.

[0004] For example, Patent Document 1 discloses that when a nanosecond laser with a wavelength of 266 to 1064 nm is irradiated onto a cutting tool, the peak power density (0.02 GW / cm) is about two orders of magnitude lower than that of general laser peening. 2 ) and Al 2 O 3 It is described in detail that the layer peels off. The peak power density is calculated as follows: pulse energy [J] / (pulse width [s] × spot area [cm 2 ])

[0005] It is generally known that the compressive residual stress imparted by laser peening correlates with the peak power density, and it is believed that the surface treatment method described in Patent Document 1 is unable to impart compressive residual stress to the surface layer of the tool substrate. 2 O 3 Peeling of the layer can cause problems such as a significant decrease in wear resistance during cutting, where the cutting edge becomes very hot.

[0006] Furthermore, Patent Document 2 describes a pulsed laser surface treatment method in which a cutting tool having a Ti-based hard coating (nitride, carbide, carbonitride) placed in a liquid atmosphere that is transparent to the laser is peened with a nanosecond pulsed laser. Such films (layers) other than oxides are difficult to peel off by laser peening, so the problem of coating peeling can be avoided, but on the other hand, the types of tools that can be applied and the cutting conditions, etc. are limited.

[0007] Furthermore, Patent Documents 3 and 4 describe a method in which a black tape or paint is applied as a protective layer on the hard coating of a cutting tool, and then a nanosecond or picosecond pulse laser with an infrared wavelength is irradiated from the black tape or paint in water to perform laser peening. 2 O 3 It is possible to impart high compressive residual stresses to the tool surface without delaminating.

[0008] Japanese Patent Application Laid-Open No. 2012-223808 Japanese Patent No. 4087349 Special Publication No. 2020-525301 Special Publication No. 2022-545909

[0009] However, in Patent Document 1, the Al of the hard coating 2 O 3In the case of Patent Document 2, oxide layers such as a layer peel off, while in Patent Document 2, there is no oxide layer, making it difficult to improve the wear resistance of the cutting tool in either case. Furthermore, in Patent Documents 3 and 4, a protective layer is first applied to the hard coating, followed by laser peening, and then the protective layer must be removed, a complex process that complicates the manufacturing process and increases manufacturing costs. Furthermore, the protective layer attenuates the impact of the laser peening, reducing the compressive residual stress imparted to the tool surface.

[0010] An object of the present invention is to provide a cutting tool manufacturing method that can manufacture a cutting tool having excellent chipping resistance and wear resistance through a simple process, and to provide the cutting tool.

[0011] In order to solve the above problems, the present invention provides the following means.

[0012] [Aspect 1 of the Present Invention] A method for manufacturing a cutting tool, comprising: a film-forming step of forming a hard coating having at least an oxide layer on the surface of a tool substrate made of sintered alloy; and an ultraviolet laser peening step of directly irradiating the hard coating with a pulsed laser having a wavelength of 190 nm to 380 nm and a pulse width of 30 fs to 2 ps in a gas atmosphere, wherein the ultraviolet laser peening step imparts compressive residual stress to a surface layer of the tool substrate directly below the oxide layer, while leaving the oxide layer on the hard coating.

[0013] In one embodiment of the present invention, a tool substrate (hereinafter sometimes referred to as workpiece) on which a hard coating has been formed is irradiated with a short-pulse laser having a pulse width of 30 fs (femtoseconds) or more and 2 ps (picoseconds) or less, which is shorter than conventional techniques. This increases the peak power density of the laser while suppressing thermal effects, allowing a large impact force to be applied to the workpiece surface, even in a gas such as air or an inert gas, thereby imparting large compressive residual stress. This process is known as ultrashort-pulse laser peening, a technique in which shock waves are generated in the workpiece by the mechanical reaction of the explosive diffusion of plasma generated by slight processing of the workpiece surface irradiated with a laser. This generates crystal defects such as plastic deformation and dislocations, thereby imparting compressive residual stress to the workpiece surface.

[0014] As a result of extensive research into hard-coated cutting tools, the inventors of the present invention have come to the following findings: In an ultraviolet laser peening process, a pulsed laser having a wavelength of 190 nm to 380 nm and a pulse width of 30 fs to 2 ps, i.e., a short-pulse laser with an ultraviolet wavelength, is directly irradiated onto a hard coating in a gas atmosphere. It has been found that this makes it possible to impart a compressive residual stress of 1 GPa or more (i.e., a residual stress of -1 GPa or less) to the surface layer of the tool substrate located below the oxide layer of the hard coating without peeling off the oxide layer.

[0015] The reason why the ultraviolet laser peening process can impart large compressive residual stress to the surface layer of the tool substrate while leaving an oxide layer on the hard coating is believed to be as follows. For the sake of convenience, Al is used as an example of an oxide layer below. 2 O 3 A TiCN layer is used as an example of a lower layer that is disposed below the oxide layer of the hard coating.

[0016] Al, an insulator 2 O 3 For example, in the case of a single crystal, the band gap of the Al layer is large at about 8 eV, and even if a laser with a pulse width of nanoseconds or more is used, even a quadruple wave (a laser with a wavelength 1 / 4 times that of a YAG laser) cannot reach this wavelength of 266 nm (4.66 eV). For this reason, in the conventional laser peening process, a part of the laser is 2 O 3 The laser penetrates the AlN layer and causes laser peening at the interface with the underlying TiCN layer. 2 O 3 The layers are likely to peel off.

[0017] In contrast, in the embodiment of the present invention, by using an ultraviolet pulse laser (ultraviolet femtosecond laser), the photon energy is increased several times by multiphoton absorption, and Al 2 O 3 Without penetrating the layer, Al 2 O 3It is believed that this makes it possible to generate laser peening on the surface of the layer. In addition, experimental results have shown that an infrared pulse laser (infrared femtosecond laser) with an infrared wavelength can 2 O 3 The delamination of the layers could not be prevented.

[0018] As described above, in the cutting tool manufacturing method according to the embodiment of the present invention and the cutting tool manufactured thereby, it is possible to form Al in the hard coating through a simple manufacturing process without providing a protective layer on the hard coating. 2 O 3 This allows a large compressive residual stress to be stably imparted to the surface layer of the tool substrate while leaving an oxide layer such as a SiO 2 layer. Therefore, the oxide layer can stably enhance wear resistance, and the large compressive residual stress can improve fracture resistance. In other words, according to this aspect of the present invention, a cutting tool with excellent fracture resistance and wear resistance can be manufactured using a simple process. This also reduces the manufacturing cost of the cutting tool.

[0019] The reason why the wavelength of the pulse laser is set to 190 nm or more and 380 nm or less in the ultraviolet laser peening process is as follows: The shorter the wavelength, the lower the laser transmittance of the oxide layer. Therefore, in order to implement this embodiment of the present invention, it is advantageous for the wavelength of the laser beam to be as short as possible within the ultraviolet range (400 nm or less). However, if the wavelength is less than 190 nm, the laser beam will be absorbed by the atmosphere (gas), making laser peening in the atmosphere difficult. In other words, if the wavelength is less than 190 nm, the laser beam will fall into the vacuum ultraviolet range, where it will attenuate in the atmosphere, and laser peening in the atmosphere may not be possible. For this reason, the lower limit of the wavelength is set to 190 nm.

[0020] Furthermore, if the wavelength is 380 nm or less, the laser transmittance of the oxide layer can be stably kept low, laser peening can be generated on the surface of the oxide layer, and peeling of the oxide layer can be stably suppressed.

[0021] [Aspect 2 of the Present Invention] The method for manufacturing a cutting tool according to Aspect 1, wherein the ultraviolet laser peening step involves irradiating a pulsed laser having a pulse width of 0.1 ps or more and less than 1 ps.

[0022] When the pulsed laser used in the ultraviolet laser peening process has an ultraviolet wavelength and a pulse width within the above-mentioned range, it is possible to impart a higher compressive residual stress to the surface layer of the tool substrate while leaving a stable oxide layer on the hard coating, thereby further improving the chipping resistance and wear resistance of the cutting tool.

[0023] [Aspect 3 of the Present Invention] The method for manufacturing a cutting tool according to Aspect 1 or 2, wherein in the ultraviolet laser peening step, the pulsed laser is scanned along a cutting edge disposed on a ridge line portion of the tool substrate.

[0024] In this case, by scanning the pulsed laser parallel to the cutting edge, compressive residual stress can be uniformly imparted to the cutting edge along the cutting edge length direction, thereby more stably improving chipping resistance.

[0025] This laser treatment also creates groove-like irregularities along the cutting edge on the surface of the oxide layer. The texture effect of the groove-like irregularities along the laser scanning line makes it easier to retain the coolant used during cutting, keeping the cutting edge temperature low and further improving wear resistance.

[0026] A fourth aspect of the present invention is a cutting tool comprising a tool base made of a sintered alloy, a cutting edge disposed on a ridge line portion of the tool base, a rake face disposed adjacent to the cutting edge, and a hard coating disposed on the surface of the tool base over at least the cutting edge and the rake face, wherein the hard coating has an overall thickness of 25 μm or less and has at least an oxide layer, the oxide layer being exposed on the surface of the hard coating over a range of at least 0.2 mm from the cutting edge toward the rake face in a direction perpendicular to the cutting edge, and wherein a portion of the surface layer of the tool base disposed directly below the oxide layer has a residual stress of −1 GPa or less.

[0027] The cutting tool according to the present invention can be manufactured by the above-described cutting tool manufacturing method. This cutting tool has an oxide layer remaining on the hard coating, and a high compressive residual stress is imparted to a portion of the surface layer of the tool substrate located directly below the oxide layer. This consistently improves wear resistance and chipping resistance, extending tool life. Furthermore, the present invention is not limited to specific types of tools or cutting conditions.

[0028] The reason why the total thickness of the hard coating is set to 25 μm or less is to stably prevent the hard coating from peeling off due to self-destruction.

[0029] In another embodiment of the present invention, laser peening is performed on the surface of the tool substrate from above the hard coating, thereby exposing an oxide layer on the surface of the hard coating after the laser treatment. The reason why this oxide layer is exposed on the surface of the hard coating in a range of at least 0.2 mm from the cutting edge toward the rake face is as follows.

[0030] Since chipping of the cutting edge during cutting is likely to occur in the area of ​​the cutting edge that directly contacts (cuts into) the workpiece, it is necessary to impart compressive residual stress to at least this area. Many common cutting tools have a maximum feed rate of 0.2 mm or more in the recommended cutting conditions listed in their catalogs. Therefore, in this embodiment of the present invention, laser peening is performed over an area of ​​at least 0.2 mm from the cutting edge toward the rake face, thereby stably increasing the cutting edge strength in this area.

[0031] Specifically, the residual stress in the portion of the surface layer of the tool substrate located directly below the oxide layer is set to -1 GPa or less (i.e., the compressive residual stress is 1 GPa or more), which makes it possible to significantly improve the fracture resistance of the cutting tool.

[0032] [Aspect 5 of the Present Invention] The cutting tool according to Aspect 4, wherein the oxide layer has groove-like irregularities arranged in a portion exposed on the surface of the hard coating.

[0033] In this case, groove-like irregularities are formed in the oxide layer exposed on the surface of the hard coating. The groove-like irregularities are formed on the surface of the oxide layer along, for example, the laser scanning line. The texture effect of these groove-like irregularities makes it easier to retain the coolant used during cutting, keeping the cutting edge temperature low and further improving the wear resistance of the cutting tool.

[0034] According to the above aspects of the present invention, it is possible to provide a cutting tool manufacturing method that can manufacture a cutting tool having excellent fracture resistance and wear resistance through a simple process, and the cutting tool.

[0035] Fig. 1 is a perspective view showing a cutting tool of this embodiment. Fig. 2 is a cross-sectional view showing an enlarged view of the vicinity of the cutting edge of the cutting tool of this embodiment. Fig. 3 is a flow diagram illustrating a method for manufacturing the cutting tool of this embodiment. Fig. 4 is a cross-sectional view showing a portion of the cutting tool, specifically, Fig. 4(a) is a cross-sectional view showing the vicinity of the hard coating after the film-forming process, Fig. 4(b) is a cross-sectional view illustrating the ultraviolet laser peening process of this embodiment, and Fig. 4(c) is a cross-sectional view illustrating a conventional laser peening process. Fig. 5 is an image showing an enlarged view of the surface of the oxide layer of the hard coating.

[0036] A cutting tool 10 and a manufacturing method for the cutting tool 10 according to one embodiment of the present invention will be described with reference to the drawings. The cutting tool 10 according to this embodiment is a cutting insert. Although not specifically shown, the cutting tool 10 according to this embodiment is used, for example, in an indexable cutting tool that performs turning (cutting) on ​​a workpiece such as a metal.

[0037] 1, the cutting tool 10 of this embodiment is plate-shaped. Specifically, the cutting tool 10 is polygonal, and in the illustrated example, it is square. However, the cutting tool 10 may be polygonal or disc-shaped, other than square.

[0038] In this embodiment, the direction in which the central axis C of the cutting tool 10 extends, i.e., the direction parallel to the central axis C, is referred to as the axial direction. In a plan view of the cutting tool 10, the central axis C is located at the center of the cutting tool 10. The central axis C extends along the thickness direction of the cutting tool 10. The direction perpendicular to the central axis C is referred to as the radial direction. Within the radial direction, the direction approaching the central axis C is referred to as the radially inner direction, and the direction away from the central axis C is referred to as the radially outer direction. The direction going around the central axis C is referred to as the circumferential direction.

[0039] 2 , the cutting tool 10 of this embodiment includes a tool base 1 made of a sintered alloy, a cutting edge 3 arranged on a ridge line portion of the tool base 1, a rake face 5 arranged adjacent to the cutting edge 3, a flank 6 arranged adjacent to the cutting edge 3, and a hard coating 2 arranged on the surface of the tool base 1 over at least the cutting edge 3 and the rake face 5. That is, the cutting tool 10 of this embodiment is a hard-coated cutting insert in which the hard coating 2 is coated on the tool base 1 (i.e., a hard-coated cutting tool, a surface-coated cutting tool).

[0040] As shown in FIG. 1 , the cutting tool 10 includes a pair of plate surfaces 10a, 10b, an outer peripheral surface 10c, and a through hole 10d. The pair of plate surfaces 10a, 10b are polygonal and face the axial direction of the central axis C. In this embodiment, the pair of plate surfaces 10a, 10b are each rectangular. The pair of plate surfaces 10a, 10b includes one plate surface (upper surface) 10a and the other plate surface (lower surface) 10b. The one plate surface 10a and the other plate surface 10b are spaced apart from each other in the axial direction and face opposite directions from each other in the axial direction.

[0041] In this embodiment, the axial direction from the other plate surface 10b to one plate surface 10a is referred to as the "one axial side," and the direction from one plate surface 10a to the other plate surface 10b is referred to as the "other axial side." The axial direction may also be referred to as the "up-down direction." In this case, the one axial side corresponds to the upper side, and the other axial side corresponds to the lower side. Of the pair of plate surfaces 10a, 10b, at least one plate surface 10a has a portion (such as a corner) that faces a workpiece (not shown) during cutting.

[0042] Of the pair of plate surfaces 10a, 10b, at least one plate surface 10a has a rake face 5 disposed thereon. The rake face 5 constitutes at least a portion of the plate surface 10a. In this embodiment, the rake faces 5 are disposed at at least two of the four corner portions located on the periphery of the plate surface 10a. The two corner portions are disposed at positions that are 180° rotationally symmetrical to each other about the central axis C.

[0043] As shown in Figure 2, the rake face 5 has a land portion 5a and an inclined portion 5b. The land portion 5a is a portion of the rake face 5 that is connected to the cutting edge 3. The land portion 5a is disposed radially inward of the cutting edge 3. In this embodiment, the land portion 5a is an inclined surface that inclines toward the other axial side (downward) as it extends radially inward from the cutting edge 3. The land portion 5a may also be a flat surface that extends in a direction perpendicular to the central axis C.

[0044] The inclined portion 5b is a portion of the rake face 5 that is located radially inward of the land portion 5a. The inclined portion 5b is connected to the radially inner end of the land portion 5a. The inclined portion 5b is an inclined surface that slopes toward the other axial side (downward) as it extends radially inward from the land portion 5a. The amount of axial displacement of the inclined portion 5b per unit length along the radial direction is greater than the amount of axial displacement of the land portion 5a. In other words, the inclination of the inclined portion 5b with respect to an imaginary plane (not shown) perpendicular to the center axis C is greater than the inclination of the land portion 5a with respect to the imaginary plane.

[0045] As shown in Fig. 1, the outer peripheral surface 10c is connected to the pair of plate surfaces 10a, 10b and faces radially outward. Both axial ends of the outer peripheral surface 10c are connected to the pair of plate surfaces 10a, 10b. Specifically, one axial end of the outer peripheral surface 10c is connected to one plate surface 10a. The other axial end of the outer peripheral surface 10c is connected to the other plate surface 10b. The outer peripheral surface 10c extends over the entire circumferential direction of the cutting tool 10.

[0046] A flank 6 is arranged on the outer peripheral surface 10c. That is, the cutting tool 10 has the flank 6. The flank 6 constitutes at least a part of the outer peripheral surface 10c. The flank 6 is arranged in a portion of the outer peripheral surface 10c adjacent to each rake face 5. The flank 6 is arranged adjacent to the cutting edge 3.

[0047] The through hole 10d passes through the cutting tool 10 in the axial direction. The through hole 10d opens to the pair of plate surfaces 10a, 10b and extends in the axial direction. The central axis of the through hole 10d is arranged coaxially with the central axis C. In the illustrated example, the through hole 10d is a circular hole. A fastening member such as a protrusion of a clamp piece or a clamp screw (not shown) is inserted into the through hole 10d. The fastening member detachably fixes the cutting tool 10 to an insert mounting seat of a holder (not shown).

[0048] The cutting edges 3 are arranged at the ridges where the rake face 5 and the flank 6 are connected, that is, at the intersecting ridges of the rake face 5 and the flank 6. In this embodiment, the cutting edges 3 are arranged at at least two of the four corners located on the periphery of the plate surface 10a. As shown in FIG. 2, in this embodiment, the cutting edges 3 have a round honing. Note that the cutting edges 3 may have other honing shapes, such as chamfer honing. Furthermore, the cutting edges 3 do not necessarily have to have a honing shape.

[0049] As shown in FIG. 1 , the cutting edge 3 has a corner cutting edge portion 3a and a pair of straight cutting edges 3b. The corner cutting edge portion 3a has a convex curved shape that protrudes radially outward. The straight cutting edge portion 3b is linear and connected to the corner cutting edge portion 3a. In this embodiment, the pair of straight cutting edges 3b are connected to both ends of the corner cutting edge portion 3a in the cutting edge length direction. The cutting edge length direction is the direction in which the cutting edge 3 extends, specifically, the direction in which each cutting edge portion 3a, 3b of the cutting edge 3 extends. The corner cutting edge portion 3a and the pair of straight cutting edges 3b form a generally V-shape when viewed in the axial direction.

[0050] As shown in FIG. 2, the cutting edge 3 is composed of the ridges (intersecting ridges) of the tool base 1 and the portions of the hard coating 2 that are coated on the ridges.

[0051] The tool substrate 1 has the same shape as the cutting tool 10 described above. The tool substrate 1 is made of a sintered alloy having at least one hard phase selected from carbides, nitrides, and mutual solid solutions of metals of Groups 4, 5, and 6 of the periodic table, and a binder phase having a weight ratio of 2 to 15% and containing Ni, Co, or a Ni-Co alloy as a main component. In this embodiment, the tool substrate 1 is made of a WC-based cemented carbide. However, the tool substrate 1 may also be made of a cermet such as a TiC-based or Ti(C,N)-based cermet.

[0052] By undergoing the ultraviolet laser peening process described later, the residual stress in the surface layer 1a of the tool substrate 1 is set to, for example, -1 GPa or less, preferably -1.5 GPa or less (negative values ​​indicate compression). The lower limit of the residual stress in the surface layer 1a of the tool substrate 1 is preferably -2.0 GPa or more. More specifically, the residual stress in a portion of the surface layer 1a of the tool substrate 1 that is located directly below an oxide layer (described later) of the hard coating 2 is, for example, -1 GPa or less, preferably -1.5 GPa or less, and the lower limit of this residual stress is preferably -2.0 GPa or more. Note that the "surface layer 1a of the tool substrate 1" in this embodiment refers to a surface layer portion of the tool substrate 1 that is at least 1 μm deep from the surface of the tool substrate 1 (the interface with the hard coating 2). In this embodiment, the residual stress may also be referred to as the residual stress of WC grains, etc.

[0053] The hard coating 2 is formed on the surface (outer surface) of the tool substrate 1 by chemical vapor deposition (CVD). The hard coating 2 is disposed on a region of the surface of the tool substrate 1 that includes at least the cutting edge 3 and the rake face 5. In this embodiment, the hard coating 2 is disposed on at least the cutting edge 3, the rake face 5, and the flank 6. The hard coating 2 may also be formed on the entire surface of the tool substrate 1.

[0054] The hard coating 2 has a laminated structure of multiple layers or a single layer, and has at least an oxide layer. 2 O 3 , ZrO 2 , TiO 2 , V.O. 2 In this embodiment, the oxide layer is Al 2 O 3The oxide layer has a thickness (film thickness) of, for example, 1 μm or more. The total film thickness of the hard coating 2 is, for example, 25 μm or less. The total film thickness of the hard coating 2 is preferably 5 μm or more. If the total film thickness of the hard coating 2 is less than 5 μm, crater wear may be more likely to progress.

[0055] When the hard coating 2 has a laminated structure of multiple layers, the layers other than the oxide layer are composed of, for example, carbide, nitride, carbonitride, or boride. In this embodiment, as shown in FIG. 4( a), a typical example of the hard coating 2 having a laminated structure is a hard coating having a TiCN layer as a lower layer 21 disposed on the surface of the tool substrate 1 and an AlCN layer as an upper layer (oxide layer) 22. 2 O 3 The thickness of each layer may be, for example, a TiCN layer (lower layer 21) and an AlN layer. 2 O 3 The TiN layer (outermost layer 23) is 1 μm thick, for example.

[0056] Although not shown, an intermediate layer of a Ti compound (TiC) having a thickness of about 0.1 μm is formed between the surface of the tool substrate 1 and the lower layer 21, and between the lower layer 21 and the upper layer 22. x N y O z ) (x+y+z=1), which reduces delamination during cutting.

[0057] Here, a description will be given of a method for manufacturing the cutting tool 10. As shown in Fig. 3, the method for manufacturing the cutting tool 10 of this embodiment includes a sintering step S1, a film forming step S2, and an ultraviolet laser peening step S3.

[0058] In the sintering step S1, raw material powder is press-molded to produce a green compact having the shape of the tool base 1, and then the green compact is sintered. The green compact is an intermediate compact that is compacted during the manufacturing process of the tool base 1. In this embodiment, the green compact is plate-shaped, specifically a polygonal plate-shaped. In this embodiment, the raw material powder is a mixed powder or the like that contains WC as a hard phase component and Ni, Co, or a Ni—Co alloy as a binder phase component.

[0059] In the film-forming step S2, a hard coating 2 having at least an oxide layer is formed on the surface of a sintered alloy tool substrate 1. More specifically, the hard coating 2 is formed by chemical vapor deposition (CVD) on at least the portions of the surface of the tool substrate 1 where the cutting edge 3, rake face 5, and flank 6 are located.

[0060] In this embodiment, as shown in FIG. 4( a ), the hard coating 2 is made up of a plurality of layers, and on the surface of the tool substrate 1 , there is a lower layer 21 made of a TiCN layer, an Al 2 O 3 An upper layer 22 made of a TiN layer (oxide layer) and an outermost layer 23 made of a TiN layer are formed in this order. In the following description, the cutting tool 10 in which the surface of the tool substrate 1 is coated with the hard coating 2 may be referred to as a workpiece.

[0061] As shown in Figures 3 and 4(b), in the ultraviolet laser peening step S3, a pulsed laser L is irradiated onto at least the cutting edge 3 and rake face 5 (i.e., the cutting edge) of the workpiece. Specifically, in the ultraviolet laser peening step S3, a pulsed laser L having a wavelength of 190 nm to 380 nm and a pulse width of 30 fs (femtoseconds) to 2 ps (picoseconds) is directly irradiated onto the hard coating 2 in a gas, such as air or an inert gas. This ultraviolet laser peening step S3 imparts compressive residual stress to the surface layer 1a of the tool substrate 1 directly below the oxide layer, while leaving the oxide layer (upper layer 22) on the hard coating 2. Preferably, in the ultraviolet laser peening step S3, a pulsed laser L having a pulse width of 0.1 ps to less than 1 ps is irradiated onto the cutting edge of the workpiece.

[0062] 1, in the ultraviolet laser peening step S3, a pulsed laser L is scanned along the cutting edge 3 arranged on the ridge line of the tool base body 1. Specifically, the cutting edge including the straight cutting edge 3b is laser-scanned with the pulsed laser L in a linear manner parallel to the straight cutting edge 3b, and the cutting edge including the corner cutting edge 3a is laser-scanned with the pulsed laser L in a curved manner parallel to the corner cutting edge 3a.

[0063] 4( b), in the ultraviolet laser peening step S3, the portion of the outermost layer 23 that has been irradiated with the pulsed laser L is removed by laser ablation. On the other hand, the upper layer 22 made of an oxide layer has high resistance to laser ablation by the pulsed laser L of this embodiment, and therefore, although the surface portion of the upper layer 22 is slightly laser-processed, most of the portion other than the surface portion remains as is in the hard coating 2.

[0064] 5 is an enlarged view of the surface of the oxide layer (upper layer 22) of the hard coating 2 laser-processed by the ultraviolet laser peening step S3. By the ultraviolet laser peening step S3, groove-like irregularities 22a extending along the laser scanning direction LS are formed on the surface of the oxide layer. The groove-like irregularities 22a have a plurality of grooves and a plurality of ribs extending along the cutting edge length direction of the cutting edge 3. The grooves and ribs are alternately arranged in a direction perpendicular to the cutting edge 3. In other words, the cutting tool 10 of this embodiment has groove-like irregularities 22a arranged in the portion of the oxide layer (upper layer 22) exposed on the surface of the hard coating 2.

[0065] Furthermore, the ultraviolet laser peening step S3 imparts a residual stress of, for example, −1 GPa or less, preferably −1.5 GPa or less to the surface layer 1a of the tool substrate 1 located directly below the upper oxide layer 22. The lower limit of the residual stress is preferably −2.0 GPa or more.

[0066] A high-energy pulsed laser L is suitable for the ultraviolet laser peening step S3 of this embodiment, and from this viewpoint, a laser that is a YAG triple harmonic (a laser with a wavelength that is 1 / 3 times the wavelength of a YAG laser) having a wavelength in the range of approximately 340 nm or more and 360 nm or less and has a pulse width of approximately 0.1 ps or more and less than 1 ps is more preferable.

[0067] 1 and 2 , the laser irradiation area A of the pulsed laser L in the ultraviolet laser peening step S3 is a strip extending along the cutting edge 3, and in this embodiment, is generally V-shaped. The lower limit of the laser irradiation area A (the width dimension) is preferably greater than the feed rate set as a cutting condition for the cutting tool 10 during cutting. Specifically, if the feed rate is greater than the laser irradiation area A, the cutting edge will cut into the workpiece to the inside of the laser irradiation area A (the side farther from the cutting edge 3), which could cause cracks or the like to occur inside the laser irradiation area A. Therefore, considering the recommended conditions in a catalog for a typical cutting tool, the laser irradiation area A needs to be at least 0.2 mm.

[0068] As described above, the TiN layer (outermost layer 23) is removed by laser ablation in accordance with the laser irradiation range A. Therefore, the oxide layer (upper layer 22) is exposed on the surface of the hard coating 2 in a range A of at least 0.2 mm from the cutting edge 3 toward the rake face 5 in the direction perpendicular to the cutting edge 3.

[0069] On the other hand, if the laser irradiation range A is excessively large, the TiN layer (outermost layer 23), which is provided for the purpose of enhancing the aesthetic appearance of the external design, will be removed by laser ablation, resulting in a noticeable deterioration in aesthetics. Therefore, the laser irradiation range A is preferably about 1.5 times the feed rate when the tool is in use. More preferably, the range in which the oxide layer is exposed on the surface of the hard coating due to laser irradiation is 0.6 mm or less. For general cutting tools, the maximum feed rate under cutting conditions is 0.6 mm or less, and it is considered sufficient to impart compressive residual stress within this range. Furthermore, if the laser irradiation range is wide, the processing time increases, which may result in a decrease in production efficiency.

[0070] Specifically, in this embodiment, a pulsed laser beam L is irradiated onto a laser irradiation area A of the workpiece, covering the cutting edge 3, the land portion 5a, and the radially outer end of the inclined portion 5b. More specifically, the pulsed laser beam L is scanned over the laser irradiation area A as shown by hatching using a galvanometer scanner and Fθ lens unit (not shown). The processing atmosphere at this time is air or an arbitrary gas. The arbitrary gas may be, for example, an inert gas that suppresses oxidation.

[0071] The cutting tool 10 and the manufacturing method of the present embodiment described above provide the following advantageous effects. In this embodiment, a tool substrate 1 (hereinafter sometimes referred to as a workpiece) on which a hard coating 2 is formed is irradiated with a short-pulse laser L having a pulse width of 30 fs (femtoseconds) or more and 2 ps (picoseconds) or less, which is shorter than conventional pulse widths. This increases the peak power density of the laser while suppressing thermal effects, thereby enabling a large impact force to be applied to the workpiece surface, even in a gas such as air or an inert gas, thereby imparting large compressive residual stress. This process is known as ultrashort-pulse laser peening, which is a technique for imparting compressive residual stress to the workpiece surface by generating shock waves due to the mechanical reaction generated when plasma explosively diffuses by slightly processing the surface of the workpiece irradiated with a laser. This generates crystal defects such as plastic deformation and dislocations, thereby imparting compressive residual stress to the workpiece surface.

[0072] As a result of extensive research into the hard-coated cutting tool 10, the inventors of the present invention have come to the following findings: In the ultraviolet laser peening step S3, a pulsed laser L having a wavelength of 190 nm to 380 nm and a pulse width of 30 fs to 2 ps, i.e., a short-pulse laser L having an ultraviolet wavelength, is directly irradiated onto the hard coating 2 in a gas. It has been found that this makes it possible to impart a compressive residual stress of 1 GPa or more (i.e., a residual stress of −1 GPa or less) to the surface layer 1a of the tool substrate 1 located below the oxide layer (upper layer 22) of the hard coating 2 without peeling off the oxide layer.

[0073] The reason why the ultraviolet laser peening step S3 can impart a large compressive residual stress to the surface layer 1a of the tool substrate 1 while leaving an oxide layer on the hard coating 2 is considered to be as follows. 2 O 3 The layer (oxide layer) has a large band gap of about 8 eV in the case of a single crystal, and even if a laser with a pulse width of nanoseconds or more is used, even if a quadruple wave (a laser with a wavelength 1 / 4 times that of a YAG laser) is used, the wavelength is 266 nm (4.66 eV), which cannot be reached. For this reason, in the conventional laser peening process, as shown in Figure 4(c), a part of the laser is irradiated with Al. 2 O 3 The laser penetrates the AlN layer and causes laser peening at the interface with the underlying TiCN layer. 2 O 3 The layers are likely to peel off.

[0074] In contrast, in the present embodiment shown in FIG. 4B, by using an ultraviolet pulse laser (ultraviolet femtosecond laser) L, the photon energy is increased several times by multiphoton absorption, and Al 2 O 3 Without penetrating the layer, Al 2 O 3 It is believed that this makes it possible to generate laser peening on the surface of the Al layer. As a result of the experiment, it was found that an infrared pulse laser (infrared femtosecond laser) with an infrared wavelength can effectively peen Al layers, as in the case of Figure 4(c) described above. 2 O 3 The delamination of the layers could not be prevented.

[0075] As described above, in the method for manufacturing the cutting tool 10 of this embodiment and the cutting tool 10 manufactured by the method, it is possible to form Al on the hard coating 2 through a simple manufacturing process without providing a protective layer on the hard coating 2. 2 O 3This allows a large compressive residual stress to be stably imparted to the surface layer 1a of the tool substrate 1 while leaving an oxide layer such as a SiO 2 layer. As a result, the oxide layer can stably enhance wear resistance, and the large compressive residual stress can improve fracture resistance. That is, according to this embodiment, a cutting tool 10 with excellent fracture resistance and wear resistance can be manufactured by a simple process. This also reduces the manufacturing cost of the cutting tool 10.

[0076] The reason why the wavelength of the pulsed laser L is set to 190 nm or more and 380 nm or less in the ultraviolet laser peening step S3 is as follows: The shorter the wavelength, the lower the laser transmittance of the oxide layer. Therefore, for implementing the present invention, it is advantageous for the wavelength of the laser beam to be as short as possible within the ultraviolet range (400 nm or less). However, if the wavelength is below 190 nm, the laser beam will be absorbed by the atmosphere (gas), making laser peening in the atmosphere difficult. In other words, if the wavelength is below 190 nm, the laser beam will fall into the vacuum ultraviolet range, where it will attenuate in the atmosphere, and laser peening in the atmosphere may not be possible. For this reason, the lower limit of the wavelength is set to 190 nm.

[0077] Furthermore, if the wavelength is 380 nm or less, the laser transmittance of the oxide layer can be stably kept low, laser peening can be generated on the surface of the oxide layer, and peeling of the oxide layer can be stably suppressed.

[0078] In this embodiment, the ultraviolet laser peening step S3 irradiates a pulsed laser L having a pulse width of 30 fs or more and 2 ps or less, preferably 0.1 ps or more and less than 1 ps. If the pulsed laser L used in the ultraviolet laser peening step S3 has an ultraviolet wavelength and a pulse width within the above-mentioned range, it becomes possible to impart a higher compressive residual stress to the surface layer 1 a of the tool substrate 1 while leaving a stable oxide layer in the hard coating 2. Therefore, the chipping resistance and wear resistance of the cutting tool 10 can be further improved.

[0079] In this embodiment, in the ultraviolet laser peening step S3, the pulsed laser L is scanned along the cutting edge 3 disposed on the ridge line of the tool base body 1. In this case, by scanning the pulsed laser L parallel to the cutting edge 3, compressive residual stress can be uniformly imparted to the cutting edge along the cutting length direction of the cutting edge 3. Therefore, the fracture resistance can be more stably improved.

[0080] Furthermore, this laser treatment forms groove-like irregularities 22a on the surface of the oxide layer along the cutting edge 3. The texture effect of the groove-like irregularities 22a along the laser scanning line makes it easier to retain the coolant (cooling water) used during cutting, keeping the cutting edge temperature low and further improving wear resistance.

[0081] Furthermore, in the cutting tool 10 of this embodiment, the overall film thickness of the hard coating 2 is 25 μm or less, the oxide layer (upper layer 22) of the hard coating 2 is exposed on the surface of the hard coating 2 in a range A of at least 0.2 mm from the cutting edge 3 toward the rake face 5 in a direction perpendicular to the cutting edge 3, and the residual stress of the portion of the surface layer 1 a of the tool substrate 1 located directly below the oxide layer is −1 GPa or less.

[0082] The cutting tool 10 of this embodiment can be manufactured by the above-described method for manufacturing the cutting tool 10. In this cutting tool 10, an oxide layer remains on the hard coating 2, and a high compressive residual stress is imparted to a portion of the surface layer 1a of the tool substrate 1 located directly below the oxide layer. This consistently improves wear resistance and fracture resistance, thereby extending the tool life. Furthermore, the present invention is not likely to limit the types of tools to which it can be applied, nor the cutting conditions.

[0083] The reason why the total thickness of the hard coating 2 is set to 25 μm or less is to stably prevent the hard coating 2 from peeling off due to self-destruction.

[0084] In this embodiment, laser peening is performed on the surface layer 1a of the tool substrate 1 from above the hard coating 2, so that an oxide layer is exposed on the surface of the hard coating 2 after the laser treatment. The reason why this oxide layer is exposed on the surface of the hard coating 2 in a range A of at least 0.2 mm from the cutting edge 3 toward the rake face 5 is as follows.

[0085] Since chipping of the cutting edge during cutting is likely to occur in the area of ​​the cutting edge that directly contacts (cuts into) the workpiece, it is necessary to impart compressive residual stress to at least this area. Many common cutting tools have a maximum feed rate of 0.2 mm or more in the recommended cutting conditions listed in their catalogs. Therefore, in this embodiment, laser peening is performed on a range A extending from the cutting edge 3 toward the rake face 5 by at least 0.2 mm, thereby stably increasing the cutting edge strength in this area.

[0086] Specifically, the residual stress in the portion of the surface layer 1a of the tool substrate 1 located directly below the oxide layer is set to -1 GPa or less (i.e., the compressive residual stress is 1 GPa or more), which makes it possible to significantly improve the chipping resistance of the cutting tool 10.

[0087] In this embodiment, the oxide layer (upper layer 22) has groove-like asperities 22a arranged in the portion exposed on the surface of the hard coating 2. In this case, the groove-like asperities 22a are formed in the oxide layer exposed on the surface of the hard coating 2. The groove-like asperities 22a are formed on the surface of the oxide layer, for example, along the laser scanning line. The texture effect of these groove-like asperities 22a makes it easier to retain the coolant used during cutting, and the cutting edge temperature is kept low, thereby further improving the wear resistance of the cutting tool 10.

[0088] The present invention is not limited to the above-described embodiment, and the configuration can be changed within the scope of the present invention, as described below.

[0089] In the above-described embodiment, the oxide layer of the upper layer 22 of the hard coating 2 is Al 2 O 3 The oxide layer may be made of any material that can ensure wear resistance, such as Al. 2 O 3 ZrO other than 2 , TiO 2 , V.O. 2 Alternatively, an oxide layer such as TiN may be used. The lower layer 21 is not limited to a TiCN layer. The outermost layer 23 made of a TiN layer does not necessarily have to be provided.

[0090] In the above embodiment, an example was given in which the cutting tool 10 is used as an indexable cutting tool, but this is not limiting. The cutting tool 10 may be used, for example, as an indexable drill or indexable end mill that performs milling (cutting) on ​​a workpiece. Furthermore, while an example was given in which the cutting tool 10 is a cutting insert, this is not limiting. The cutting tool 10 may be, for example, a solid-type cutting tool, a drill, an end mill, a reamer, or other cutting tools.

[0091] The present invention may be combined with the various configurations described in the above-described embodiments and modifications, and may also include additions, omissions, substitutions, and other modifications within the scope of the present invention. The present invention is not limited to the above-described embodiments, but is limited only by the claims.

[0092] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.

[0093] As cutting tools serving as examples and comparative examples of the present invention, several cutting tools were prepared by carrying out the film-forming step S2 of the manufacturing method for the cutting tool 10 described above. The cutting tools 10 are cutting inserts having a shape conforming to JIS standard CNMG120408. The tool substrates 1 of these cutting tools were made of WC-based cemented carbide, and a hard coating 2 was formed on the surface of the tool substrate 1 by a CVD method. Specifically, a TiCN layer of 5 μm was formed as the lower layer 21 of the hard coating 2, and an AlN layer was formed as the upper layer 22. 2 O 3 A layer of 3 μm was formed, and a TiN layer of 1 μm was formed as the outermost layer 23 .

[0094] Next, in Examples 1 to 5 of the present invention and Comparative Example 1, laser peening was performed on each cutting tool after the coating step S2 in the atmosphere by scanning a pulse laser L having a wavelength of 320 nm or 343 nm at equal intervals along the cutting edge 3 with a pulse width in the range of 0.03 ps (30 fs) to 5 ps, and setting the laser irradiation range A = 0.5 mm from the tip of the cutting edge 3 to the inside of the rake face 5. The interval and scanning speed of the laser scanning lines at this time were set to be equal to or greater than 0.5 mm after the laser irradiation. 2 O 3The value was adjusted so that the layer remained with a thickness of about 1.5 to 2.0 μm.

[0095] In addition, as a comparative example 2, a pulse laser having a wavelength of 1030 nm and a pulse width of 1 ps was irradiated onto the cutting tool after the film-forming step S2. 2 O 3 The Al layer was peeled off. 2 O 3 It was not possible to process the layer to a predetermined depth (to stop the process midway). In addition, a cutting tool that was not subjected to laser peening was used as Comparative Example 3.

[0096] The wavelength (nm), pulse width (ps), and pulse energy (mJ) of the pulse laser during the laser peening treatment in Examples 1 to 5 and Comparative Examples 1 and 2, and the Al after the laser peening treatment 2 O 3 The remaining film thickness (μm) of the Al layer is shown in Table 1 below. 2 O 3 The remaining thickness of the layer was measured by cutting the laser-processed surface of the workpiece and taking an electron microscope image of the cross section.

[0097]

[0098] In Table 1, the pulse energy differs for each condition because the wavelength conversion efficiency to ultraviolet laser is higher as the pulse is shorter. 2 O 3 It can be seen that groove-like irregularities 22a are generated along the laser scanning line (laser scanning direction LS) on the surface of the Al layer (upper layer 22). 2 O 3 This shows that the layer was indeed laser processed.

[0099] Furthermore, for each cutting tool of the example and comparative examples, the residual stress of the WC grains in the surface layer 1a of the tool substrate 1 located directly below the laser irradiation area A was measured using the cos α method of X-ray diffraction. Specifically, the X-ray irradiation area was set to φ0.3 mm, and the residual stress was measured using the diffraction peak of WC (113) near 2θ = 154°. The measurement results are shown in Table 1.

[0100] Furthermore, for each of the cutting tools in the Examples and Comparative Examples, a fracture resistance test using a plate material and a wear resistance test using a round bar were conducted. Specifically, the fracture resistance of the cutting edge was tested by applying intermittent impacts to a 2 mm thick steel (SCM440) plate material using an NC lathe, and the wear resistance was tested by continuously cutting a round bar. In both tests, the tool life was defined as the point at which the chipping width or wear width on the flank face of the tool cutting edge exceeded 0.2 mm. The plate material test was measured by the number of impacts (times), and the round bar test was measured by the cutting time (minutes).

[0101] The cutting conditions for the plate material test and the round bar test were as follows: <Plate material test (fracture resistance confirmation test)> Cutting speed: Vc = 200 m / min Feed rate: f = 0.3 mm / rev Depth of cut: ap = 2.5 mm Other: The test was performed six times, and the average value of each test was used for evaluation.

[0102] <Round bar test (wear resistance confirmation test)> Cutting speed: Vc = 200 m / min Feed rate: f = 0.3 mm / rev Depth of cut: ap = 1.5 mm Other: The test was carried out once and judged.

[0103] The criteria for "judgment (evaluation)" based on each test result were as follows: A: Tool life in the plate material test was 10,000 times or more, and tool life in the round bar test was 50 minutes or more. B: Tool life in the plate material test was 8,000 times or more, and tool life in the round bar test was 45 minutes or more. C: Tool life in the plate material test was less than 8,000 times, or tool life in the round bar test was less than 45 minutes.

[0104] As shown in Table 1, Examples 1 to 5 were all judged to be "B" or higher. Specifically, in all of Examples 1 to 5, the tool life in the plate test and the tool life in the round bar test were increased compared to Comparative Example 3 (laser untreated product).

[0105] In Examples 1 to 5, the reason for the significant extension of tool life in the plate material test is believed to be due to the increase in compressive residual stress caused by the laser peening treatment. Also, the reason for the extension of tool life in the round bar test is believed to be due to the reduction of Al generated after CVD coating by the laser peening treatment. 2 O 3 The tensile residual stress in the layer was released (approaching zero), which resulted in the formation of Al due to micro-cracks during cutting of the round bar. 2 O 3 This is thought to be due to the suppression of particle shedding, the texture effect of the groove-like irregularities 22a along the laser scanning line making it easier to retain coolant and reducing the cutting edge temperature, or a combination of both. Furthermore, among Examples 1 to 5, Examples 2 and 3 in particular showed particularly significant increases in tool life in both the plate material test and the round bar test.

[0106] On the other hand, in Comparative Example 1, the compressive residual stress was not sufficiently increased, and the improvement in the tool life in the plate test was slight compared to Comparative Example 3, which was an unlaser-treated product. In Comparative Example 2, the tool life in the plate test was significantly extended due to the presence of high compressive residual stress, but the Al in the laser irradiation range A was 2 O 3 Since the layer was completely removed (peeled off), the tool life (wear resistance) in the round bar test was lower than that of Comparative Example 3, which was an unlaser-treated product.

[0107] According to the present invention, it is possible to provide a cutting tool manufacturing method that can manufacture a cutting tool having excellent fracture resistance and wear resistance through a simple process, and the cutting tool, and therefore the present invention has industrial applicability.

[0108] 1...tool substrate, 1a...surface layer, 2...hard coating, 3...cutting edge, 5...rake face, 10...cutting tool, 22...upper layer (oxide layer), 22a...groove-shaped irregularities, A...laser irradiation range, L...pulse laser, S2...film formation process, S3...ultraviolet laser peening process.

Claims

1. A method for manufacturing a cutting tool, comprising: a coating process for coating a hard coating having at least an oxide layer on the surface of a tool base made of sintered alloy; and an ultraviolet laser peening process for directly irradiating the hard coating with a pulsed laser having a wavelength of 190 nm or more and 380 nm or less and a pulse width of 30 fs or more and 2 ps or less in a gaseous state, wherein the ultraviolet laser peening process imparts compressive residual stress to the surface layer of the tool base directly below the oxide layer, while leaving the oxide layer on the hard coating.

2. The method for manufacturing a cutting tool according to claim 1, wherein the ultraviolet laser peening step irradiates a pulsed laser having a pulse width of 0.1 ps or more and less than 1 ps.

3. The method for manufacturing a cutting tool according to claim 1 or 2, wherein in the ultraviolet laser peening process, the pulsed laser is scanned along a cutting edge disposed on a ridge portion of the tool base.

4. A cutting tool comprising a tool base made of sintered alloy, a cutting edge arranged on a ridge of the tool base, a rake face arranged adjacent to the cutting edge, and a hard coating arranged on at least the cutting edge and the rake face of the surface of the tool base, wherein the hard coating has an overall thickness of 25 μm or less and has at least an oxide layer, the oxide layer being exposed on the surface of the hard coating over a range of at least 0.2 mm from the cutting edge toward the rake face in a direction perpendicular to the cutting edge, and the residual stress in a portion of the surface layer of the tool base arranged directly below the oxide layer is -1 GPa or less.

5. The cutting tool according to claim 4, wherein the oxide layer has groove-like irregularities arranged in the portion exposed on the surface of the hard coating.

Citation Information

Patent Citations

  • Method and device for laser peening

    JP2015093284A

  • Manufacturing method of cutting tool

    JP2021122935A

  • Cutting tool

    JP2021142610A

  • Cutting tool and cutting tool manufacturing method

    JP2022143008A

  • Cutting tool

    WO2020250625A1

Cited By

  • Coated tool and cutting tool

    WO2026083717A1