Fullerene derivative solution, method for producing coating film, and method for producing imaging device

The fullerene derivative solution, with carefully selected solvents based on Hansen solubility parameters, addresses the solubility challenges of fullerene derivatives, enabling the formation of thicker coating films and enhancing the performance of photoelectric conversion elements and imaging devices.

WO2024203157A1PCT designated stage expired Publication Date: 2024-10-03PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/008993
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-08
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Fullerene derivatives are difficult to dissolve in solvents, making it challenging to achieve sufficient film thickness in coating processes, which is essential for industrial manufacturing of devices like photoelectric conversion elements.

Method used

A fullerene derivative solution is developed, comprising a fullerene derivative, a first solvent with a boiling point of 200°C or less, and a second solvent with a boiling point of 100°C or less, where the Hansen solubility parameters of the solvents are specifically tailored to enhance solubility and drying speed, ensuring film thickness and industrial usability.

Benefits of technology

The solution effectively increases the solubility and drying speed of fullerene derivatives, allowing for the formation of thicker, high-quality coating films, thereby improving the device characteristics of photoelectric conversion elements and imaging devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024008993_03102024_PF_FP_ABST
    Figure JP2024008993_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The fullerene derivative solution contains a fullerene derivative, a first solvent, and a second solvent. The boiling point of the first solvent is 200°C or less. The boiling point of the second solvent is 100°C or less. The ranges 17.8 ≦ δD1 ≦ 18.9, 4.4 ≦ δP1 ≦ 4.7, and 4.8 ≦ δH1 ≦ 6.9 are satisfied where δD1 represents the dispersion force term in the Hansen solubility parameters of the first solvent, δP1 represents the polarity term in the Hansen solubility parameters of the first solvent, and δH1 represents the hydrogen bond term in the Hansen solubility parameters of the first solvent. The volume of the first solvent is larger than the volume of the second solvent.
Need to check novelty before this filing date? Find Prior Art

Description

Fullerene derivative solution, method for producing coated film, and method for producing imaging device

[0001] The present disclosure relates to a fullerene derivative solution, a method for producing a coating film using the fullerene derivative solution, and a method for producing an imaging device using the fullerene derivative solution.

[0002] Organic semiconductor materials possess properties and functions not found in conventional inorganic semiconductor materials such as silicon. For this reason, organic semiconductor materials have been actively researched in recent years as semiconductor materials that can realize new semiconductor devices and electronic devices.

[0003] For example, research has been conducted into the realization of photoelectric conversion elements by forming organic semiconductor materials into thin films and using them as photoelectric conversion materials. Photoelectric conversion elements using organic material thin films can be used as image sensors such as solid-state imaging devices by extracting charges generated by light as electrical signals (see, for example, Patent Document 1).

[0004] In addition, in a photoelectric conversion element using an organic semiconductor material, phenyl C 61 Fullerene derivatives, such as butyric acid methyl ester (

[60] PCBM), are widely used as acceptor materials. Fullerene derivatives tend to aggregate and are difficult to dissolve in solvents, and research on the solubility of fullerene derivatives has been reported (see, for example, Non-Patent Document 1).

[0005] Patent No. 5969843

[0006] Chun I Wang et. al. , “Solubility of C60 and PCBM in Organic Solvents”, J. Phys. Chem. B, American Chemical Society, 2015, Vol. 119, pp. 14496-14504Charles M. Hansen, “THE THREE DIMENSIONAL SOLUBILITY PARAMETER AND SOLVENT DIFFUSION COEFFICIENT Their Importance In Surface Coating Formulation”, COPENHAGEN DANISH TECHNICAL PRESS, 1967

[0007] As described above, fullerene derivatives are difficult to dissolve in solvents. On the other hand, there is a demand for industrially useful fullerene derivative solutions that can ensure a sufficient film thickness when forming a coating film containing a fullerene derivative using a coating process in industrial device manufacturing processes.

[0008] Therefore, the present disclosure provides an industrially useful fullerene derivative solution, a method for producing a coating film, and a method for producing an imaging device.

[0009] A fullerene derivative solution according to one embodiment of the present disclosure includes a fullerene derivative, a first solvent, and a second solvent. The boiling point of the first solvent is 200°C or lower. The boiling point of the second solvent is 100°C or lower. The following relationships are satisfied: 17.8 ≦ δD1 ≦ 18.9, 4.4 ≦ δP1 ≦ 4.7, and 4.8 ≦ δH1 ≦ 6.9, where δD1 represents the dispersion force term in the Hansen solubility parameter of the first solvent, δP1 represents the polar term in the Hansen solubility parameter of the first solvent, and δH1 represents the hydrogen bonding term in the Hansen solubility parameter of the first solvent. The volume of the first solvent is larger than the volume of the second solvent.

[0010] Furthermore, a method for producing a coating film according to one aspect of the present disclosure includes preparing the fullerene derivative solution and applying the fullerene derivative solution onto a substrate to form a coating film.

[0011] According to the present disclosure, it is possible to provide an industrially useful fullerene derivative solution, a method for producing a coating film, and a method for producing an imaging device.

[0012] Fig. 1 is a schematic cross-sectional view showing a photoelectric conversion element according to embodiment 2. Fig. 2 is a flowchart showing a method for manufacturing a coating film used in the photoelectric conversion element according to embodiment 2.

[0013] (Summary of the Present Disclosure) As an overview of one embodiment of the present disclosure, examples of a fullerene derivative solution, a method for producing a coating film, and a method for producing an imaging device according to the present disclosure are described below.

[0014] A fullerene derivative solution according to a first aspect of the present disclosure includes a fullerene derivative, a first solvent, and a second solvent. The boiling point of the first solvent is 200°C or lower. The boiling point of the second solvent is 100°C or lower. The following relationships are satisfied: 17.8 ≦ δD1 ≦ 18.9, 4.4 ≦ δP1 ≦ 4.7, and 4.8 ≦ δH1 ≦ 6.9, where δD1 represents the dispersion force term in the Hansen solubility parameter of the first solvent, δP1 represents the polarity term in the Hansen solubility parameter of the first solvent, and δH1 represents the hydrogen bonding term in the Hansen solubility parameter of the first solvent. The volume of the first solvent is greater than the volume of the second solvent. In other words, the ratio of the volume of the first solvent to the total volume of the first solvent and the second solvent is greater than the ratio of the volume of the second solvent to the total volume.

[0015] This allows the drying speed during application to be increased while maintaining the solubility of the fullerene derivative, thereby ensuring a sufficient film thickness when forming a coating film using the fullerene derivative solution, thereby realizing an industrially useful fullerene derivative solution.

[0016] Furthermore, for example, the fullerene derivative solution according to the second aspect of the present disclosure may be the fullerene derivative solution according to the first aspect, in which δD1>δD2 is satisfied, where δD2 represents the dispersion force term in the Hansen solubility parameter of the second solvent.

[0017] This makes it easier for the first solvent to cover the fullerene derivative, and the solubility of the fullerene derivative can be maintained even when the fullerene derivative solution contains the second solvent.

[0018] Furthermore, for example, the fullerene derivative solution according to the third aspect of the present disclosure may be the fullerene derivative solution according to the first or second aspect, in which δH1>δH2 is satisfied, where δH2 represents the hydrogen bond term in the Hansen solubility parameter of the second solvent.

[0019] This makes it more difficult for the second solvent to hydrogen bond with the fullerene derivative than the first solvent, and the solubility of the fullerene derivative in the fullerene derivative solution can be maintained even when the fullerene derivative solution contains the second solvent.

[0020] Furthermore, for example, the fullerene derivative solution according to the fourth aspect of the present disclosure is the fullerene derivative solution according to any one of the first to third aspects, and may satisfy the following conditions: 15.5≦δD2≦17.5, 4.0≦δP2≦6.0, 3.0≦δH2≦6.0, where δD2 represents the dispersion force term in the Hansen solubility parameter of the second solvent, δP2 represents the polarity term in the Hansen solubility parameter of the second solvent, and δH2 represents the hydrogen bond term in the Hansen solubility parameter of the second solvent.

[0021] This allows the solubility of the fullerene derivative to be maintained even when the fullerene derivative solution contains a second solvent.

[0022] Furthermore, for example, the fullerene derivative solution according to the fifth aspect of the present disclosure may be the fullerene derivative solution according to any one of the first to fourth aspects, in which the first solvent is an oxygen-containing aromatic compound.

[0023] This is an example of an embodiment.

[0024] Furthermore, for example, the fullerene derivative solution according to the sixth aspect of the present disclosure may be the fullerene derivative solution according to any one of the first to fifth aspects, in which the first solvent is anisole, 2,3-dihydrobenzofuran, or 2-methoxytoluene.

[0025] This makes it possible to realize a fullerene derivative solution in which the fullerene derivative is highly soluble and has low toxicity.

[0026] Furthermore, for example, the fullerene derivative solution according to the seventh aspect of the present disclosure may be the fullerene derivative solution according to any one of the first to sixth aspects, in which the second solvent is an oxygen-containing aliphatic compound.

[0027] This is an example of an embodiment.

[0028] Furthermore, for example, the fullerene derivative solution according to the eighth aspect of the present disclosure may be the fullerene derivative solution according to any one of the first to seventh aspects, in which the second solvent is 2-methyltetrahydrofuran.

[0029] This makes it possible to realize a fullerene derivative solution in which the fullerene derivative has high solubility and low toxicity.

[0030] Furthermore, for example, the fullerene derivative solution according to the ninth aspect of the present disclosure may be the fullerene derivative solution according to any one of the first to eighth aspects, and the concentration of the fullerene derivative may be 20 mg / ml or more.

[0031] This makes it possible to form a thicker coating film using the fullerene derivative solution.

[0032] Furthermore, a method for producing a coating film according to a tenth aspect of the present disclosure includes preparing a fullerene derivative solution according to any one of the first to ninth aspects, and applying the fullerene derivative solution onto a substrate to form a coating film.

[0033] As a result, since the coating film is formed using the fullerene derivative solution, the thickness of the coating film can be ensured.

[0034] Furthermore, a method for producing a coating film according to an eleventh aspect of the present disclosure is the method for producing a coating film according to the tenth aspect, and the coating film may be formed as a photoelectric conversion layer of a photoelectric conversion element.

[0035] This ensures the film thickness of the photoelectric conversion layer, and improves the device characteristics of the photoelectric conversion element.

[0036] Furthermore, a method for producing a coating film according to a twelfth aspect of the present disclosure is the method for producing a coating film according to the tenth aspect, and the coating film may be formed as a charge blocking layer of a photoelectric conversion element.

[0037] This ensures a sufficient film thickness for the charge blocking layer, thereby improving the device characteristics of the photoelectric conversion element.

[0038] Furthermore, a manufacturing method for an imaging device according to a thirteenth aspect of the present disclosure is a manufacturing method for an imaging device equipped with a photoelectric conversion element including a first electrode, a second electrode, and a photoelectric conversion layer between the first electrode and the second electrode, and includes preparing a fullerene derivative solution according to any one of the first to ninth aspects, applying the fullerene derivative solution on or above the first electrode to form a coating film, and forming the second electrode on or above the coating film.

[0039] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the drawings.

[0040] The embodiments described below are all comprehensive or specific examples. The numerical values, shapes, components, component placement and connection configurations, steps, and step sequences shown in the following embodiments are merely examples and are not intended to limit the present disclosure. Furthermore, among the components in the following embodiments, components not recited in independent claims are described as optional components, and the drawings are not necessarily strict illustrations. In the drawings, substantially identical components are denoted by the same reference numerals, and redundant descriptions may be omitted or simplified.

[0041] Furthermore, in this specification, terms indicating the relationship between elements, terms indicating the shape of elements, and numerical ranges are not expressions that only express a strict meaning, but are expressions that also include a substantially equivalent range, for example, a difference of about a few percent.

[0042] The Hansen solubility parameter is known as an index of the solubility of substances with each other, and is described, for example, in Charles M. Hansen, "Hansen Solubility Parameters: A Users Handbook", CRC Press, 2007, and Non-Patent Document 2. The Hansen solubility parameter represents solubility using three values: a dispersion force term (δD), a polar term (δP), and a hydrogen bonding term (δH). These three parameters are expressed as the coordinates of a point in a three-dimensional space called the Hansen space.

[0043] First Embodiment A fullerene derivative solution according to the present embodiment will be described below.

[0044] [Solubility of Fullerene Derivative] First, before describing the fullerene derivative solution according to the present embodiment, the results of the inventor's investigation into the solubility of fullerene derivatives in various solvents will be described.

[0045] Specifically, the inventors attempted to dissolve

[60] PCBM, a fullerene derivative, in various solvents. First, 24 mg of

[60] PCBM was weighed into a sealable glass container, and then 1 ml of solvent was added. The container was sealed and stirred at room temperature. The solvent containing

[60] PCBM was stirred for 16 hours, then the stirring was stopped and the container was left to stand for 1 hour. The presence or absence of precipitate at the bottom of the glass container was visually confirmed to determine the solubility of

[60] PCBM. In determining the solubility, if there was no precipitate, it was judged to be "soluble." If there was precipitate and the solvent was colored, it was judged to be "partially soluble." If there was precipitate and the solvent was not colored, it was judged to be "insoluble."

[0046] The solvents used were anisole, 2-methoxytoluene, 3-methoxytoluene, 4-methoxytoluene, 2,3-dihydrobenzofuran, ethyl phenyl ether, limonene, methanol, ethanol, isopropanol, acetone, cyclohexane, cyclohexanone, propylene glycol monomethyl ether acetate, butyl acetate, tetrahydrofuran, 2-methyltetrahydrofuran, dihydropyran, 2-methyl-1,3-dioxane, and N-methyl-2-pyrrolidone. These solvents were selected because they are less toxic than chlorobenzene and chloroform, as used in Non-Patent Document 1, and are easy to use industrially.

[0047] For each of the solvents listed above, the type of solvent, the Hansen solubility parameter of the solvent, the boiling point of the solvent, and the results of the solubility assessment are shown in Table 1.

[0048]

[0049] As shown in Table 1, anisole, 2-methoxytoluene, and 2,3-dihydrobenzofuran were able to dissolve

[60] PCBM.

[0050] Limonene, 3-methoxytoluene, 4-methoxytoluene and ethyl phenyl ether were also able to partially dissolve

[60] PCBM.

[0051] Methanol, ethanol, isopropanol, acetone, cyclohexane, cyclohexanone, propylene glycol monomethyl ether acetate, butyl acetate, tetrahydrofuran, 2-methyltetrahydrofuran, dihydropyran, 2-methyl-1,3-dioxane, and N-methyl-2-pyrrolidone were unable to dissolve

[60] PCBM.

[0052] The results in Table 1 show that solvents whose Hansen solubility parameters satisfy the following conditions: 17.8≦dispersion force term (δD)≦18.9, 4.4≦polarity term (δP)≦4.7, 4.8≦hydrogen bond term (δH)≦6.9 have high solubility of fullerene derivatives.

[0053] [Fullerene Derivative Solution] Next, the fullerene derivative solution according to this embodiment will be described in detail.

[0054] The fullerene derivative solution according to this embodiment includes a fullerene derivative, a first solvent, and a second solvent. In the fullerene derivative solution, the fullerene derivative is dissolved in a mixed solvent containing the first solvent and the second solvent. The main components of the solvent in the fullerene derivative solution are, for example, the first solvent and the second solvent. Here, the term "main component" means a content of more than 50 vol%. The content of the main component of the solvent in the fullerene derivative solution may be 80 vol% or more, or may be 90 vol% or more. For example, the first solvent and the second solvent used in the fullerene derivative solution are each one type, but at least one of them may be two or more types.

[0055] The fullerene derivative solution is used, for example, to form a coating film containing the fullerene derivative by applying the fullerene derivative solution and removing the solvent, thereby forming a coating film containing the fullerene derivative.

[0056] Examples of fullerene derivatives include

[60] PCBM and phenyl C 71 Butyric acid methyl ester (

[70] PCBM), phenyl C 61 Butyric acid butyl ester (

[60] PCBB), phenyl C 61 Butyric acid octyl ester (

[60] PCBO), phenyl C 61 Dodecyl butyrate (

[60] PCBD), bis-phenyl C 61 Butyric acid methyl ester (Bis-PCBM) and indene C 60 Examples of the fullerene derivative include a bis-adduct (ICBA). The fullerene derivative contains, for example, an ester structure, and has enhanced solubility in a solvent compared to fullerene. The fullerene derivative solution may contain two or more types of fullerene derivatives.

[0057] The concentration of the fullerene derivative in the fullerene derivative solution is, for example, 20 mg / ml or more, which makes it easier to form a thick film using the fullerene derivative solution.

[0058] The first solvent is a solvent that has high solubility for the fullerene derivative. Specifically, when the Hansen solubility parameters of the first solvent are δD1, δP1, and δH1, respectively, the dispersion force term, polar term, and hydrogen bond term of the first solvent are δD1, δP1, and δH1, respectively, and the first solvent is a solvent whose δD1, δP1, and δH1 satisfy predetermined conditions.

[0059] In the fullerene derivative solution according to the present embodiment, 17.8≦δD1≦18.9, 4.4≦δP1≦4.7, and 4.8≦δH1≦6.9 are satisfied. As can be seen from the results of the investigation into the solubility of the fullerene derivative described above, the solubility of the fullerene derivative in the first solvent is thereby increased, and therefore the solubility of the fullerene derivative in the fullerene derivative solution can be increased.

[0060] The first solvent does not contain, for example, a halogen element. The first solvent is, for example, an oxygen-containing aromatic compound. The oxygen-containing aromatic compound is a compound in which at least some of the hydrogen atoms in an aromatic hydrocarbon are substituted with a substituent containing an oxygen atom. The aromatic hydrocarbon is, for example, benzene. The substituent containing an oxygen atom is, for example, an —OR group (alkoxy group, R represents an aliphatic hydrocarbon group). The oxygen-containing aromatic compound may have a phenoxy structure. Note that in the oxygen-containing aromatic compound, some of the hydrogen atoms in the aromatic hydrocarbon may be substituted with a substituent not containing an oxygen atom, such as a hydrocarbon group.

[0061] From the viewpoint of low toxicity and high solubility of the fullerene derivative, the first solvent may be anisole, 2,3-dihydrobenzofuran, or 2-methoxytoluene.

[0062] The second solvent has a boiling point lower than that of the first solvent. The boiling point of the first solvent is 200°C or lower. The boiling point of the second solvent is 100°C or lower. This increases the drying speed of the fullerene derivative solution, making it possible to form a coating film with a larger thickness. From the viewpoint of ease of handling, the boiling points of the first solvent and the second solvent may each be 50°C or higher.

[0063] Furthermore, when the dispersion force term is δD2, the polarity term is δP2, and the hydrogen bonding term is δH2 among the Hansen solubility parameters of the second solvent, a solvent whose δD2, δP2, and δH2 satisfy predetermined conditions may be used as the second solvent.

[0064] For example, in the fullerene derivative solution according to the present embodiment, δD1>δD2 is satisfied, which makes it easier for the first solvent to cover the periphery of the fullerene derivative, thereby maintaining the solubility of the fullerene derivative in the fullerene derivative solution.

[0065] Furthermore, for example, in the fullerene derivative solution according to the present embodiment, δH1>δH2 is satisfied, which makes it more difficult for the second solvent to hydrogen bond with the fullerene derivative than the first solvent, thereby maintaining the solubility of the fullerene derivative in the fullerene derivative solution.

[0066] Furthermore, for example, in the fullerene derivative solution according to this embodiment, the following conditions are satisfied: 15.5≦δD2≦17.5, 4.0≦δP2≦6.0, and 3.0≦δH2≦6.0. This also makes it possible to maintain the solubility of the fullerene derivative in the fullerene derivative solution.

[0067] The second solvent does not contain, for example, a halogen element. The second solvent is, for example, an oxygen-containing aliphatic compound. The oxygen-containing aliphatic compound is a compound that contains an oxygen atom and an aliphatic hydrocarbon structure, but does not contain an aromatic ring structure. Examples of the oxygen-containing aliphatic compound include ethers, ketones, esters, and alcohols. Among these, the oxygen-containing aliphatic compound may be an ether. The ether may be a cyclic ether. In the ether, some of the hydrogen atoms may be substituted with an aliphatic hydrocarbon group such as a methyl group. This can lower δD2 and δH2.

[0068] The second solvent may be 2-methyltetrahydrofuran, from the viewpoints of low toxicity, low boiling point, and ease of maintaining the solubility of the fullerene derivative in the fullerene derivative solution.

[0069] In the fullerene derivative solution according to this embodiment, the volume of the first solvent is larger than the volume of the second solvent. In other words, the ratio of the volume of the first solvent to the total volume of the first solvent and the second solvent is larger than the ratio of the volume of the second solvent to the total volume. This can enhance the solubility of the fullerene derivative. Furthermore, the volume percentage, which is the ratio of the volume of the first solvent to the total volume of the first solvent and the second solvent, may be 60% or more. Furthermore, from the viewpoint of ensuring the thickness of the film formed using the fullerene derivative, the volume percentage, which is the ratio of the volume of the first solvent to the total volume of the first solvent and the second solvent, may be 90% or less, or may be 80% or less. When multiple types of first solvents are used in the fullerene derivative solution, the volume of the first solvent is the sum of the volumes of the multiple types of first solvents. Similarly, when multiple types of second solvents are used in the fullerene derivative solution, the volume of the second solvent is the sum of the volumes of the multiple types of second solvents.

[0070] The volume percentage, which is the ratio of the volume of the first solvent to the total volume of all solvents in the fullerene derivative solution, may be, for example, greater than 50% and not less than 60%, and the volume percentage, which is the ratio of the volume of the first solvent to the total volume of all solvents in the fullerene derivative solution, may be, for example, not more than 90%, or not more than 80%.

[0071] Furthermore, the fullerene derivative solution according to the present embodiment may contain components other than the fullerene derivative, the first solvent, and the second solvent. The fullerene derivative solution according to the present embodiment may contain, for example, a donor material such as a donor organic semiconductor material. This allows the fullerene derivative to act as an acceptor material, making it possible to easily form a mixed film with a bulk heterostructure using the fullerene derivative solution.

[0072] The fullerene derivative solution is prepared, for example, as follows.

[0073] First, the fullerene derivative is weighed and placed in a container. If necessary, other solute materials, such as a donor material, are also weighed and placed in the container. Next, one or more first solvents and one or more second solvents are added to the container in a predetermined volume ratio, the container is sealed, and the mixture is stirred at room temperature. This yields a fullerene derivative solution. The container may be heated during stirring. Alternatively, only the one or more first solvents may be added to the container and stirred, followed by the addition of the one or more second solvents.

[0074] (Embodiment 2) Next, embodiment 2 will be described. In embodiment 2, a photoelectric conversion element using a coating film formed from the fullerene derivative solution according to embodiment 1 will be described. In the following description of embodiment 2, differences from embodiment 1 will be mainly described, and descriptions of commonalities will be omitted or simplified.

[0075] The photoelectric conversion element according to the present embodiment is, for example, a charge readout type photoelectric conversion element. Fig. 1 is a schematic cross-sectional view showing a photoelectric conversion element 10 according to the present embodiment.

[0076] As shown in FIG. 1 , the photoelectric conversion element 10 is supported on a support substrate 1. The photoelectric conversion element 10 includes a pair of electrodes: a first electrode 2 and a second electrode 6 disposed opposite the first electrode 2; and a photoelectric conversion layer 4 located between the first electrode 2 and the second electrode 6. The photoelectric conversion element 10 further includes a charge blocking layer 3 located between the first electrode 2 and the photoelectric conversion layer 4, and a charge blocking layer 5 located between the second electrode 6 and the photoelectric conversion layer 4. One of the charge blocking layer 3 and the charge blocking layer 5 is an electron blocking layer, and the other is a hole blocking layer. Note that the photoelectric conversion element 10 is only required to include at least the first electrode 2, the second electrode 6, and the photoelectric conversion layer 4; it is not necessary to include at least one of the charge blocking layer 3 and the charge blocking layer 5.

[0077] The photoelectric conversion element 10 is used, for example, in an imaging device. In an imaging device using the photoelectric conversion element 10, for example, each of a plurality of pixels included in the imaging device has a photoelectric conversion unit configured by the photoelectric conversion element 10. The use of the photoelectric conversion element 10 is not particularly limited, and it may be used in an optical sensor or a solar cell.

[0078] Hereinafter, each component of the photoelectric conversion element 10 according to this embodiment will be described.

[0079] The support substrate 1 may be any substrate that is commonly used in photoelectric conversion elements, such as a glass substrate, a semiconductor substrate, or a plastic substrate.

[0080] The first electrode 2 is formed from a metal, a metal nitride, a metal oxide, or polysilicon that has been made conductive. Examples of metals include aluminum, copper, titanium, and tungsten. An example of a method for making polysilicon conductive is to dope it with impurities.

[0081] The second electrode 6 is a transparent electrode formed of, for example, a transparent conductive material. Examples of the material of the second electrode 6 include transparent conductive oxide (TCO), indium tin oxide (ITO), indium zinc oxide (IZO), aluminum-doped zinc oxide (AZO), fluorine-doped tin oxide (FTO), and SnO. 2 and TiO 2 and the like. The second electrode 6 may be made of a TCO and a metal material such as aluminum (Al) or gold (Au), either singly or in combination, depending on the desired transmittance. In the photoelectric conversion element 10, for example, light transmitted through the second electrode 6 is incident on the photoelectric conversion layer 4. In this specification, the term "transparent" means that the photoelectric conversion layer 4 transmits at least a portion of light of a wavelength that can be absorbed, and does not necessarily transmit light over the entire wavelength range. In this specification, for convenience, electromagnetic waves in general, including visible light, infrared light, and ultraviolet light, are referred to as "light."

[0082] The materials of the first electrode 2 and the second electrode 6 are not limited to the above-mentioned conductive materials, and other materials may be used. For example, the first electrode 2 may be a transparent electrode. In this case, light transmitted through the first electrode 2 may be incident on the photoelectric conversion layer 4.

[0083] Various methods are used to fabricate the first electrode 2 and the second electrode 6 depending on the materials used. For example, when ITO is used, methods such as an electron beam method, a sputtering method, a resistance heating vapor deposition method, a chemical reaction method such as a sol-gel method, or a method of applying a dispersion of indium tin oxide may be used. In this case, to fabricate the first electrode 2 and the second electrode 6, after forming the ITO film, UV-ozone treatment, plasma treatment, or the like may be further performed.

[0084] A bias voltage is applied to the first electrode 2 and the second electrode 6, for example, via wiring (not shown). For example, the polarity of the bias voltage is determined so that, of the charges generated in the photoelectric conversion layer 4, electrons move to the second electrode 6 and holes move to the first electrode 2. An example in which electrons move to the second electrode 6 and holes move to the first electrode 2 will be described below. Note that the bias voltage may also be set so that, of the charges generated in the photoelectric conversion layer 4, holes move to the second electrode 6 and electrons move to the first electrode 2.

[0085] The photoelectric conversion layer 4 includes a donor material and an acceptor material. The photoelectric conversion layer 4 is fabricated using, for example, organic semiconductor materials as the donor and acceptor materials. The photoelectric conversion layer 4 can be fabricated by, for example, a wet method such as a coating method using spin coating or a dry method such as a vacuum deposition method. The vacuum deposition method is a method in which a layer material is vaporized by heating under vacuum and deposited on a substrate. The charge blocking layer 3 and the charge blocking layer 5 can also be fabricated using a method similar to that for the photoelectric conversion layer 4.

[0086] The photoelectric conversion layer 4 is, for example, a mixed film with a bulk heterostructure containing a donor material such as a donor organic semiconductor material and an acceptor material such as an acceptor organic semiconductor material. The photoelectric conversion layer 4 may have a laminated structure in which a layer of the donor material and a layer of the acceptor material are laminated.

[0087] The photoelectric conversion layer 4 generates electron-hole pairs therein upon irradiation with light. The generated electron-hole pairs are separated into electrons and holes by the electric field applied to the photoelectric conversion layer 4, and each migrates to the first electrode 2 side or the second electrode 6 side according to the electric field. Here, of the electron-hole pairs generated by absorbing light, the material that donates the electron to the other material is a donor material, and the material that accepts the electron is an acceptor material. When two different types of organic semiconductors are used, which material serves as the donor material and which as the acceptor material is generally determined by the relative positions of the HOMO (Highest-Occupied-Molecular-Orbital) and LUMO (Lowest-Unoccupied-Molecular-Orbital) energy levels of the two types of organic semiconductors at their contact interface. Specifically, a material having a shallower LUMO energy level that accepts electrons is a donor material, and a material having a deeper LUMO energy level is an acceptor material.

[0088] The photoelectric conversion layer 4 can be easily formed as a thin film by including a donor organic semiconductor material and an acceptor organic semiconductor material. Specific examples of donor organic semiconductor materials and acceptor organic semiconductor materials are given below.

[0089] Examples of donor organic semiconductor materials include triarylamine compounds, benzidine compounds, pyrazoline compounds, styrylamine compounds, hydrazone compounds, triphenylmethane compounds, carbazole compounds, polysilane compounds, thiophene compounds, phthalocyanine compounds, naphthalocyanine compounds, subphthalocyanine compounds, cyanine compounds, merocyanine compounds, oxonol compounds, polyamine compounds, indole compounds, pyrrole compounds, pyrazole compounds, polyarylene compounds, fused aromatic carbon ring compounds (e.g., naphthalene derivatives, anthracene derivatives, phenanthrene derivatives, tetracene derivatives, pyrene derivatives, perylene derivatives, and fluoranthene derivatives), and metal complexes having nitrogen-containing heterocyclic compounds as ligands. However, without being limited thereto, any organic compound having a smaller ionization potential than the organic compound used as the acceptor organic semiconductor material may be used as the donor organic semiconductor material.

[0090] Examples of the acceptor organic semiconductor material include fullerene derivatives, fullerenes (e.g., C60 fullerene and C70 fullerene), fused aromatic carbocyclic compounds (e.g., naphthalene derivatives, anthracene derivatives, phenanthrene derivatives, tetracene derivatives, pyrene derivatives, perylene derivatives, and fluoranthene derivatives), 5- to 7-membered heterocyclic compounds containing a nitrogen atom, an oxygen atom, or a sulfur atom (e.g., pyridine, pyrazine, pyrimidine, pyridazine, triazine, quinoline, quinoxaline, quinazoline, phthalazine, cinnoline, isoquinoline, pteridine, acridine, phenazine, Examples of the acceptor organic semiconductor material include metal complexes having, as a ligand, phenanthroline, tetrazole, pyrazole, imidazole, thiazole, oxazole, indazole, benzimidazole, benzotriazole, benzoxazole, benzothiazole, carbazole, purine, triazolopyridazine, triazolopyrimidine, tetrazaindene, oxadiazole, imidazopyridine, pyrrolidine, pyrrolopyridine, thiadiazolopyridine, dibenzazepine, tribenzazepine, etc.), polyarylene compounds, fluorene compounds, cyclopentadiene compounds, silyl compounds, and nitrogen-containing heterocyclic compounds. However, the acceptor organic semiconductor material is not limited thereto, and any organic compound having a larger electron affinity than the organic compound used as the donor organic semiconductor material may be used as the acceptor organic semiconductor material.

[0091] The photoelectric conversion layer 4 can be formed using the fullerene derivative solution according to embodiment 1. In this case, the acceptor organic semiconductor material is a fullerene derivative.

[0092] The donor organic semiconductor material and the acceptor organic semiconductor material are not limited to the above examples. Low-molecular-weight organic compounds and high-molecular-weight organic compounds may be used as the donor organic semiconductor material and the acceptor organic semiconductor material constituting the photoelectric conversion layer 4, as long as they are organic compounds that can be formed into a film as a photoelectric conversion layer by either a dry method or a wet method.

[0093] The charge blocking layers 3 and 5 suppress the injection of charges from the electrodes into the photoelectric conversion layer 4. By providing the charge blocking layers 3 and 5, it is possible to suppress the injection of charges from the electrodes into the photoelectric conversion layer 4, and to reduce noise signals that adversely affect the signal-to-noise ratio (SN ratio).

[0094] Specifically, the charge blocking layer 3 is an electron blocking layer provided to reduce dark current caused by electrons injected from the first electrode 2. The charge blocking layer 3 suppresses electrons from being injected from the first electrode 2 into the photoelectric conversion layer 4. The charge blocking layer 3 also has the function of transporting holes generated in the photoelectric conversion layer 4 to the first electrode 2.

[0095] The charge blocking layer 5 is a hole blocking layer provided to reduce dark current caused by holes injected from the second electrode 6. The charge blocking layer 5 suppresses holes from being injected from the second electrode 6 into the photoelectric conversion layer 4. The charge blocking layer 5 also has the function of transporting electrons generated in the photoelectric conversion layer 4 to the second electrode 6.

[0096] The charge blocking layer 3 and the charge blocking layer 5 are formed of, for example, an organic semiconductor material having HOMO and LUMO energy levels that act as a barrier to the movement of charges from the electrodes to the photoelectric conversion layer 4 .

[0097] The charge blocking layer 3 and the charge blocking layer 5 can be formed using the fullerene derivative solution according to the embodiment 1. In this case, the organic semiconductor material is a fullerene derivative.

[0098] The materials of charge blocking layer 3 and charge blocking layer 5 are not limited to organic semiconductor materials, but may be inorganic semiconductor materials such as oxide semiconductors and nitride semiconductors, or composite materials thereof.

[0099] In the photoelectric conversion element 10, when holes of the charges generated in the photoelectric conversion layer 4 move to the second electrode 6 and electrons move to the first electrode 2, the charge blocking layer 3 becomes a hole blocking layer and the charge blocking layer 5 becomes an electron blocking layer.

[0100] In the photoelectric conversion element 10, at least one of the photoelectric conversion layer 4, the charge blocking layer 3 and the charge blocking layer 5 is a coating film formed using the fullerene derivative solution according to the first embodiment.

[0101] 2 is a flowchart of a method for manufacturing a coating film used in the photoelectric conversion element 10 according to this embodiment. As shown in FIG. 2, first, a fullerene derivative solution containing a fullerene derivative, a first solvent, and a second solvent is prepared (step S11). As described in the first embodiment, the fullerene derivative solution can be obtained, for example, by adding the first solvent and the second solvent to the fullerene derivative and stirring the mixture. When the coating film is formed as the photoelectric conversion layer 4, the fullerene derivative solution may further contain a donor material.

[0102] Next, the fullerene derivative solution prepared in step S11 is applied to a substrate to form a coating film (step S12). In this embodiment, the substrate is the layer immediately below the layer to be formed as a coating film of the fullerene derivative solution in the photoelectric conversion element 10. Specifically, the substrate is the first electrode 2, the charge blocking layer 3, or the photoelectric conversion layer 4. The method for applying the fullerene derivative solution is not particularly limited, and spin coating, inkjet coating, and coating methods using a coater are used. In this embodiment, the fullerene derivative solution is applied by spin coating, for example. For example, the support substrate 1 on which the substrate is formed is placed on the stage of a spin coater, and an amount of fullerene derivative solution corresponding to the substrate size is dropped onto the center of the substrate. After the dropping is completed, the substrate is rotated at a set rotation speed, and a coating film containing the fullerene derivative is obtained on the substrate. Furthermore, if the coating film does not completely dry during spin coating, a solvent removal process, such as heating the coating film, may be further performed.

[0103] The thickness of the coating film can be controlled by the rotation speed per hour in spin coating. Specifically, if the rotation speed per hour in spin coating is reduced, the film thickness will be thicker, and if the rotation speed per hour in spin coating is increased, the film thickness will be thinner. The rotation speed per hour in spin coating is not particularly limited, but from the viewpoint of ensuring the desired film thickness and forming a coating film with a uniform thickness, it may be 300 rpm or more and 3000 rpm or less.

[0104] In addition, the thickness of the coating film can also be increased by increasing the concentration of the fullerene derivative in the fullerene derivative solution. Furthermore, if the solvent in the fullerene derivative solution does not evaporate easily, the fullerene derivative solution tends to spread during application, resulting in a thin coating film, and it is also difficult to control the film thickness by the rotation speed per hour in spin coating. On the other hand, if the solvent in the fullerene derivative solution evaporates easily, the fullerene derivative solution dries before spreading widely, making it possible to increase the thickness of the coating film.

[0105] The fullerene derivative solution according to the first embodiment can increase the concentration of the fullerene derivative by including the first solvent, and can also increase the drying speed by including the second solvent, so that it is easy to adjust the thickness of the coating film, and for example, it is possible to form a coating film with a large thickness.

[0106] The coating film formed by the above manufacturing method does not have to be used as the photoelectric conversion layer 4, charge blocking layer 3, or charge blocking layer 5 of the photoelectric conversion element 10, and can be used as various semiconductor films. The coating film may also be formed on a substrate. The substrate may be, for example, a glass substrate made of quartz glass or alkali-free glass, or a semiconductor substrate made of a silicon wafer. The substrate may be cleaned with water or an organic solvent as needed. Before coating, organic matter adhering to the surface may be removed using a UV ozone cleaning device. This improves the wettability of the fullerene derivative solution to the substrate.

[0107] The fullerene derivative solution according to the present disclosure will be specifically described below in examples, but the present disclosure is not limited to the following examples. Specifically, a fullerene derivative solution for evaluation was prepared, and the solubility of the fullerene derivative in the fullerene derivative solution and the film thickness of a coating film formed using the fullerene derivative solution were evaluated.

[0108] (Preparation of fullerene derivative solutions) Fullerene derivative solutions in Examples and Comparative Examples were prepared. In the fullerene derivative solutions in Examples and Comparative Examples,

[60] PCBM was used as the fullerene derivative, and a naphthalocyanine compound represented by the following structural formula (1) was used as the donor material.

[0109]

[0110] [Example 1] 24 mg of

[60] PCBM was placed in a sealable glass container, and a total of 1 ml of a first solvent, anisole, and a second solvent, 2-methyltetrahydrofuran, were added to the glass container at a volume ratio of 80:20. The glass container was sealed and stirred at room temperature for 16 hours. This gave a fullerene derivative solution in Example 1.

[0111] Example 2 A fullerene derivative solution in Example 2 was obtained by carrying out the same steps as in Example 1, except that the volume ratio of anisole to 2-methyltetrahydrofuran was changed to 60:40.

[0112] Example 3 A fullerene derivative solution in Example 3 was obtained by carrying out the same steps as in Example 2, except that 6 mg of a donor material was further added to the glass container together with

[60] PCBM.

[0113] Example 4 The fullerene derivative solution in Example 4 was obtained by carrying out the same steps as in Example 1, except that the weight of

[60] PCBM placed in the glass container was changed to 48 mg and 2,3-dihydrobenzofuran was used as the first solvent.

[0114] Example 5 The fullerene derivative solution in Example 5 was obtained by carrying out the same steps as in Example 2, except that the weight of

[60] PCBM placed in the glass container was changed to 48 mg and 2,3-dihydrobenzofuran was used as the first solvent.

[0115] Comparative Example 1 A fullerene derivative solution in Comparative Example 1 was obtained by carrying out the same steps as in Example 1, except that 2-methyltetrahydrofuran was not added to the glass container and 1 ml of anisole was used as the first solvent.

[0116] Comparative Example 2 A fullerene derivative solution in Comparative Example 2 was obtained by carrying out the same steps as in Example 4, except that 2-methyltetrahydrofuran was not added to the glass container and 1 ml of 2,3-dihydrobenzofuran was used as the first solvent.

[0117] Example 6 A fullerene derivative solution in Example 6 was obtained by carrying out the same steps as in Example 2, except that tetrahydrofuran was used as the second solvent.

[0118] Example 7 The fullerene derivative solution in Example 7 was obtained by carrying out the same steps as in Example 4, except that the weight of

[60] PCBM placed in the glass container was changed to 24 mg and tetrahydrofuran was used as the second solvent.

[0119] Example 8 A fullerene derivative solution in Example 8 was obtained by carrying out the same steps as in Example 2, except that isopropanol was used as the second solvent.

[0120] (Evaluation of Solubility of Fullerene Derivative and Thickness of Coating Film) The solubility of the fullerene derivative in the obtained fullerene derivative solution was evaluated, and the thickness of the coating film formed from the fullerene derivative solution was measured.

[0121] [Evaluation of Solubility] The solubility of

[60] PCBM was judged by visually checking the presence or absence of precipitate at the bottom of the glass container for the fullerene derivative solutions in Examples 1 to 8 and Comparative Examples 1 and 2. In judging solubility, if there was no precipitate, it was judged to be "soluble," if there was precipitate and the solvent was colored, it was judged to be "partially soluble," and if there was precipitate and the solvent was not colored, it was judged to be "insoluble." The evaluation results of the solubility of the fullerene derivatives are shown in Table 2.

[0122] [Measurement of Coating Film Thickness] Coating films were formed using the fullerene derivative solutions of Examples 1 to 5 and Comparative Examples 1 and 2, and the thicknesses of the coating films were measured. To form the coating films, a 25 mm square quartz glass substrate was first placed on the stage of a spin coater, and 100 μl of the fullerene derivative solution was dropped onto the center of the quartz glass substrate. After the dropping was completed, the substrate was rotated at 500 rpm for 60 seconds to form a coating film containing the fullerene derivative on the quartz glass substrate. A portion of the formed coating film was scratched and removed, and the step in that portion was measured with a stylus-type step gauge (DEKTAK (registered trademark) stylus-type profiling system) to measure the thickness of the coating film. The measurement results of the coating film thickness are shown in Table 2.

[0123]

[0124] Table 2 also shows the composition of the fullerene derivative solution, along with the evaluation results of the solubility of the fullerene derivative and the measurement results of the thickness of the coating film.

[0125] As can be seen from Table 2, in the evaluation of the solubility of the fullerene derivative, fullerene derivative solutions in which

[60] PCBM was completely dissolved were obtained in the fullerene derivative solutions in Examples 1 to 5 and Comparative Examples 1 and 2. Furthermore, in the fullerene derivative solutions in Examples 6 to 8, although some

[60] PCBM remained dissolved, 90% or more of the

[60] PCBM was dissolved. Thus, in the fullerene derivative solutions in Examples 1 to 8, the solubility of

[60] PCBM was ensured using solvents that are less toxic than chlorobenzene, chloroform, and the like and are easily available industrially.

[0126] Furthermore, as can be seen from Table 2, in the measurement of the thickness of the coated film, the fullerene derivative solutions in Comparative Examples 1 and 2 did not contain a second solvent with a low boiling point, and therefore the thickness of the resulting coated film was thin, ranging from 55 nm to 60 nm. In contrast, the fullerene derivative solutions in Examples 1 to 5 contained a second solvent, which resulted in a thicker coating film. It can be seen that the greater the amount of second solvent in the fullerene derivative solution, the thicker the coating film can be. Furthermore, in the fullerene derivative solution in Example 3, even when a donor material was added, the thickness of the resulting coated film was thicker than when no donor material was added. Furthermore, the fullerene derivative solutions in Examples 4 and 5 contained a higher concentration of

[60] PCBM than the fullerene derivative solutions in Examples 1 and 2, and therefore the thickness of the resulting coated film was even thicker.

[0127] Although the thickness of the coating film can be increased by reducing the rotation speed per hour in spin coating, if the rotation speed per hour becomes too low, the uniformity of the thickness of the coating film decreases, and therefore there is a practical limit to how much the thickness can be increased by reducing the rotation speed per hour. With the fullerene derivative solutions in Examples 1 to 5, even when spin coating is performed at the same rotation speed per hour, thicker coating films are obtained than with the fullerene derivative solutions in Comparative Examples 1 and 2, and the thickness of the coating film can be ensured. In other words, with the fullerene derivative solutions in Examples 1 to 5, it is possible to increase the film thickness to a greater extent than with the fullerene derivative solutions in Comparative Examples 1 and 2, and the range of film thickness adjustment is greater.

[0128] As described above, it is understood that by mixing the first solvent and the second solvent and using the mixture to prepare a fullerene derivative solution, an industrially useful fullerene derivative solution can be realized.

[0129] While the fullerene derivative solution and photoelectric conversion element according to the present disclosure have been described above based on embodiments and examples, the present disclosure is not limited to these embodiments and examples. As long as they do not deviate from the gist of the present disclosure, various modifications conceivable by those skilled in the art to the embodiments and examples, as well as other forms constructed by combining some of the components of the embodiments and examples, are also included within the scope of the present disclosure.

[0130] The fullerene derivative solution according to the present disclosure can be used to form a coating film containing a fullerene derivative. Furthermore, the coating film formed using the fullerene derivative solution according to the present disclosure can be used in a photoelectric conversion element, an imaging device using the photoelectric conversion element, and the like.

[0131] REFERENCE SIGNS LIST 1 Support substrate 2 First electrode 3, 5 Charge blocking layer 4 Photoelectric conversion layer 6 Second electrode 10 Photoelectric conversion element

Claims

1. A fullerene derivative solution comprising: a fullerene derivative; a first solvent; and a second solvent, wherein the boiling point of the first solvent is 200°C or less; the boiling point of the second solvent is 100°C or less; 17.8≦δD1≦18.9, 4.4≦δP1≦4.7, and 4.8≦δH1≦6.9 are satisfied, where δD1 represents a dispersion force term in the Hansen solubility parameters of the first solvent, δP1 represents a polarity term in the Hansen solubility parameters of the first solvent, and δH1 represents a hydrogen bond term in the Hansen solubility parameters of the first solvent; and the volume of the first solvent is greater than the volume of the second solvent.

2. The fullerene derivative solution according to claim 1, wherein δD1>δD2 is satisfied, and δD2 represents the dispersion force term in the Hansen solubility parameter of the second solvent.

3. The fullerene derivative solution according to claim 1, wherein δH1>δH2 is satisfied, and δH2 represents a hydrogen bond term in the Hansen solubility parameter of the second solvent.

4. The fullerene derivative solution according to claim 1, wherein 15.5≦δD2≦17.5, 4.0≦δP2≦6.0, and 3.0≦δH2≦6.0 are satisfied, where δD2 represents the dispersion force term in the Hansen solubility parameters of the second solvent, δP2 represents the polarity term in the Hansen solubility parameters of the second solvent, and δH2 represents the hydrogen bond term in the Hansen solubility parameters of the second solvent.

5. The fullerene derivative solution according to claim 1, wherein the first solvent is an oxygen-containing aromatic compound.

6. The fullerene derivative solution according to claim 1, wherein the first solvent is anisole, 2,3-dihydrobenzofuran or 2-methoxytoluene.

7. The fullerene derivative solution according to claim 1, wherein the second solvent is an oxygen-containing aliphatic compound.

8. The fullerene derivative solution according to claim 1, wherein the second solvent is 2-methyltetrahydrofuran.

9. The fullerene derivative solution according to claim 1, wherein the concentration of the fullerene derivative is 20 mg / ml or more.

10. A method for producing a coating film, comprising: preparing a fullerene derivative solution according to any one of claims 1 to 9; and applying the fullerene derivative solution onto a substrate to form a coating film.

11. The method for producing a coating film according to claim 10, wherein the coating film is formed as a photoelectric conversion layer of a photoelectric conversion element.

12. The method for producing a coating film according to claim 10, wherein the coating film is formed as a charge blocking layer of a photoelectric conversion element.

13. A method for manufacturing an imaging device having a photoelectric conversion element including a first electrode, a second electrode, and a photoelectric conversion layer between the first electrode and the second electrode, comprising: preparing a fullerene derivative solution according to any one of claims 1 to 9; forming a coating film by applying the fullerene derivative solution on or above the first electrode; and forming the second electrode on or above the coating film.

Citation Information

Patent Citations

  • Fullerene derivative, its solution, and its membrane

    JP2009132640A

  • Photoelectric conversion element

    JP2019212763A

  • semiconductor

    JP2019518831A

  • Resist underlayer composition and pattern formation method using said composition

    JP2022166033A

  • Photovoltaic element

    WO2017159609A1