Pigment dispersion and ink composition
The pigment dispersion with a crosslinked polymer dispersant, featuring specific structural units, addresses the challenge of long-term stability by maintaining the polymer's adsorption on the pigment, thereby enhancing the ink's stability and performance.
Patent Information
- Application Number
- PCT/JP2024/009132
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-08
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional pigment dispersions in ink compositions face challenges in maintaining stability over time, requiring improved formulations to enhance long-term dispersion stability.
A pigment dispersion comprising water, a pigment, and a polymer dispersant with a crosslinked structure, specifically containing structural units represented by formulas (1) and (2), which include aromatic groups for adsorption and alkyl groups for hydrophilic/hydrophobic balance, forming a crosslinked structure to prevent desorption and agglomeration, thereby maintaining stability.
The described pigment dispersion achieves excellent stability over time due to the crosslinked structure and balanced hydrophilic/hydrophobic properties, ensuring the polymer dispersant remains adsorbed on the pigment, preventing stability decreases and maintaining effective dispersion.
Smart Images

Figure JP2024009132_03102024_PF_FP_ABST
Abstract
Description
Pigment dispersion and ink composition
[0001] The present disclosure relates to pigment dispersions and ink compositions.
[0002] Various studies have been conducted on pigment dispersions used in ink compositions. For example, Patent Document 1 listed below discloses an aqueous pigment dispersion that achieves both high levels of pigment dispersibility and dispersion stability, the aqueous pigment dispersion containing an aqueous medium, a pigment, and a polymer dispersant, wherein the polymer dispersant has at least a (meth)acrylate structural unit having a benzene ring, a (meth)acrylate structural unit having an alkyl group with 12 or more carbon atoms, and a structural unit having an ionic group, the content of the (meth)acrylate structural unit having a benzene ring in the polymer dispersant being 20 to 60% by mass and the content of the (meth)acrylate structural unit having an alkyl group with 12 or more carbon atoms being 10 to 40% by mass, and the polymer dispersant forming a crosslinked structure in the aqueous pigment dispersion.
[0003] JP 2016-069487 A
[0004] However, there are cases where it is desired to further improve the temporal stability of pigment dispersions. An object of one embodiment of the present disclosure is to provide a pigment dispersion and an ink composition having excellent temporal stability.
[0005] The present disclosure includes the following aspects: <1> A pigment dispersion containing water, a pigment, and a polymer dispersant having a crosslinked structure, wherein the polymer dispersant having a crosslinked structure further contains a structural unit represented by the following formula (1) and a structural unit represented by the following formula (2):
[0006]
[0007] In formula (1), R 1 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; R 2 represents an alkylene group having 2 to 5 carbon atoms; R 3 represents an aromatic group; 1 and X 2each independently represents —O— or —NH—, and m represents an integer of 2 or more. 4 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; R 5 represents an alkyl group having 8 or more carbon atoms; X 3 represents —O— or —NH—.
[0008] <2> The pigment dispersion according to <1>, wherein the polymer dispersant containing a crosslinked structure further contains a structural unit derived from a monomer containing an acid group, and the hydrophilic / hydrophobic ratio represented by the following formula is 8 or more: Hydrophilic / hydrophobic ratio = (mass ratio of the structural unit represented by formula (2) to the total mass of the polymer dispersant containing a crosslinked structure × R in formula (2) 2 (number of carbon atoms in the alkylene group represented by the formula (I)) / (mass ratio of structural units derived from monomers containing acid groups to the total mass of the polymer dispersant containing a crosslinked structure)
[0009] <3> The pigment dispersion according to <1> or <2>, wherein the polymer dispersant containing a crosslinked structure has an Ar valence, represented by the following formula, of 0.4 mmol / g to 2.9 mmol / g: Ar valence = (number of mmoles of structural units represented by formula (1) per 1 g of polymer dispersant containing a crosslinked structure) × (number of aromatic rings in the structural units represented by formula (1)).
[0010] <4> In formula (1), R 2 represents an alkylene group having 2 carbon atoms. <5> The pigment dispersion according to any one of <1> to <4>, wherein the polymer dispersant containing a crosslinked structure is formed by crosslinking an uncrosslinked polymer dispersant, and the uncrosslinked polymer dispersant contains a structural unit represented by formula (1), a structural unit represented by formula (2), and an acid group, and 10% to 90% of the total number of the acid groups contained therein are neutralized. <6> An ink composition comprising the pigment dispersion according to any one of <1> to <5>.
[0011] According to one embodiment of the present disclosure, a pigment dispersion and an ink composition having excellent stability over time are provided.
[0012] In this specification, a numerical range indicated using "to" means a range that includes the numerical values before and after "to" as the minimum and maximum values, respectively. In numerical ranges described in stages in this specification, the upper or lower limit value described in a certain numerical range may be replaced with the upper or lower limit value of another staged numerical range. Furthermore, in numerical ranges described in this specification, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the Examples. In this specification, when multiple substances corresponding to each component are present in the composition, the amount of each component refers to the total amount of the multiple substances present in the composition, unless otherwise specified. In this specification, a combination of two or more preferred embodiments is a more preferred embodiment. In this specification, the term "process" includes not only independent processes but also processes that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. In this specification, "(meth)acrylate" is a concept that encompasses both acrylate and methacrylate. Furthermore, "(meth)acrylic" is a concept that encompasses both acrylic and methacrylic. In the present disclosure, the singular reference of an element does not exclude the presence of a plurality unless expressly stated otherwise, unless causing a technical contradiction.
[0013] [Pigment Dispersion] The pigment dispersion of the present disclosure contains water, a pigment, and a polymer dispersant having a crosslinked structure, and the polymer dispersant having a crosslinked structure further contains a structural unit represented by the following formula (1) (hereinafter also referred to as a "formula (1) unit") and a structural unit represented by the following formula (2) (hereinafter also referred to as a "formula (2) unit"):
[0014]
[0015] In formula (1), R 1 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; R 2 represents an alkylene group having 2 to 5 carbon atoms; R 3 represents an aromatic group; 1 and X 2each independently represents —O— or —NH—, and m represents an integer of 2 or more. 4 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; R 5 represents an alkyl group having 8 or more carbon atoms; X 3 represents —O— or —NH—.
[0016] The pigment dispersion of the present disclosure has excellent stability over time, and therefore, an ink composition containing the pigment dispersion of the present disclosure (for example, an ink composition prepared by adding other components to the pigment dispersion of the present disclosure) also has excellent stability over time.
[0017] The reason why the pigment dispersion of the present disclosure has excellent stability over time is presumed to be as follows: In the pigment dispersion of the present disclosure, the pigment is dispersed in a state in which the polymer dispersant is adsorbed on the surface of the pigment. The polymer dispersant is a dispersant represented by R 3 It is believed that the polymer dispersant adsorbs to the pigment using the aromatic group represented by the formula: 2 -X 2 It is believed that this improves the affinity of the polymer dispersant for water, and as a result, the phenomenon of the polymer dispersant aggregating into a thread ball (random coil) in the aqueous pigment dispersion is suppressed. As a result, the polymer dispersant contains a formula (1) unit in which the number of repeating R -" structure (for example, alkyleneoxy structure) is 2 or more. 3 It is considered that the aromatic group represented by the formula (2) acts as an adsorbing group and is easily adsorbed to the pigment, thereby improving the dispersion stability of the pigment (i.e., the stability over time of the pigment dispersion). 5 is an alkyl group having 8 or more carbon atoms. That is, the polymer dispersant is a hydrophobic group having 8 or more carbon atoms (R 5) is included. This is thought to prevent the hydrophilicity of the polymer dispersant as a whole from becoming too high, and as a result, to prevent a decrease in the dispersion stability of the pigment (i.e., a decrease in the stability over time of the pigment dispersion). As described above, it is thought that the pigment dispersion of the present disclosure achieves excellent stability over time due to the combined effect of the crosslinked structure, the effect of the formula (1) unit, and the effect of the formula (2) unit in the polymer dispersant.
[0018] <Water> The pigment dispersion of the present disclosure contains water. The water content relative to the total amount of the pigment dispersion is preferably 40% by mass or more, more preferably 50% by mass or more, even more preferably 60% by mass or more, and still more preferably 70% by mass or more. The upper limit of the water content relative to the total amount of the pigment dispersion is, for example, 98% by mass, 95% by mass, or 90% by mass.
[0019] <Pigment> The pigment dispersion of the present disclosure contains at least one pigment. There are no particular limitations on the pigment, and it may be either an organic pigment or an inorganic pigment. Examples of the pigment include pigments described in known documents such as "Pigment Dictionary" edited by Seijiro Ito (published in 2000), "Industrial Organic Pigments" by W. Herbst and K. Hunger, and JP-A Nos. 2002-12607, 2002-188025, 2003-26978, 2003-342503, and 2015-193729.
[0020] Examples of pigments include polycyclic pigments such as azo lake pigments, azo pigments, phthalocyanine pigments, perylene pigments, perinone pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, diketopyrrolopyrrole pigments, thioindigo pigments, isoindolinone pigments, and quinophthalone pigments; organic pigments such as nitro pigments, nitroso pigments, aniline black, and daylight fluorescent pigments; and inorganic pigments such as titanium oxide, iron oxide, and carbon black. The pigment is preferably an azo pigment, a phthalocyanine pigment, an anthraquinone pigment, a quinacridone pigment, or a carbon black pigment. For details of pigments, reference may be made to the descriptions in known documents such as Japanese Patent No. 5,404,669.
[0021] In terms of hue, examples of pigments include cyan pigments, magenta pigments, yellow pigments, black pigments, and white pigments.
[0022] The content of the pigment relative to the total amount of the pigment dispersion is preferably 1% by mass to 40% by mass, more preferably 3% by mass to 30% by mass, even more preferably 5% by mass to 25% by mass, and still more preferably 10% by mass to 20% by mass.
[0023] <Polymer dispersant containing a crosslinked structure> The pigment dispersion of the present disclosure contains at least one polymer dispersant containing a crosslinked structure. The polymer dispersant containing a crosslinked structure further contains a unit of formula (1) (i.e., a structural unit represented by formula (1)) and a unit of formula (2) (i.e., a structural unit represented by formula (2)).
[0024] (Structural Unit Represented by Formula (1)) The polymer dispersant containing a crosslinked structure contains at least one unit of formula (1) (i.e., a structural unit represented by formula (1)).
[0025]
[0026] In formula (1), R 1 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; R 2 represents an alkylene group having 2 to 5 carbon atoms; R 3 represents an aromatic group; 1 and X 2 each independently represents —O— or —NH—, and m represents an integer of 2 or more.
[0027] In formula (1), R 1 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 1 is preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, more preferably a hydrogen atom, a methyl group, or an ethyl group, and even more preferably a hydrogen atom or a methyl group.
[0028] In formula (1), R 2 represents an alkylene group having 2 to 5 carbon atoms. 2is preferably an alkylene group having 2 to 4 carbon atoms, more preferably an alkylene group having 2 or 3 carbon atoms, and even more preferably an alkylene group having 2 carbon atoms.
[0029] In formula (1), R 3 represents an aromatic group. 3 The aromatic group represented by R contains at least one aromatic ring. 3 The aromatic ring in the aromatic group represented by R may be a monocyclic ring or a polycyclic ring (for example, a condensed ring). 3 The aromatic group represented by R may contain a group formed by linking monocyclic rings (for example, a biphenyl group). 3 The aromatic group represented by may contain a heteroatom (for example, an oxygen atom).
[0030] R 3 The aromatic ring in the aromatic group represented by the formula (I) may have a substituent. Examples of the substituent on the aromatic ring include linear or branched hydrocarbon groups having 1 to 30 carbon atoms (more preferably 1 to 20 carbon atoms) (e.g., linear or branched alkyl groups, linear or branched alkenyl groups, linear or branched alkynyl groups, etc.), halogen atoms, etc.
[0031] R 3 The aromatic group represented by the formula (I) preferably has 4 to 30 carbon atoms, more preferably 6 to 30 carbon atoms, even more preferably 6 to 25 carbon atoms, and still more preferably 6 to 20 carbon atoms.
[0032] R 3 The aromatic group represented by the formula (I) is preferably a phenyl group, a naphthyl group, a furyl group, a biphenyl group, or an alkylphenyl group having 7 to 30 carbon atoms (preferably 7 to 25 carbon atoms, more preferably 7 to 20 carbon atoms).
[0033] In formula (1), X 1 and X 2 Each of X independently represents —O— or —NH—. 1 and X 2 is preferably —O—.
[0034] In formula (1), m represents an integer of 2 or greater. m is preferably an integer of 2 to 30, more preferably an integer of 2 to 20, and even more preferably an integer of 2 to 10.
[0035] The content of the unit of formula (1) relative to the total amount of the polymer dispersant containing a crosslinked structure is preferably 3% by mass to 80% by mass, more preferably 5% by mass to 70% by mass, even more preferably 10% by mass to 60% by mass, and still more preferably 10% by mass to 50% by mass.
[0036] The content of the unit of formula (1) relative to the total amount of the polymer dispersant containing a crosslinked structure, excluding the crosslinked structure, is preferably 3% by mass to 80% by mass, more preferably 5% by mass to 70% by mass, even more preferably 10% by mass to 60% by mass, and still more preferably 10% by mass to 50% by mass.
[0037] The formula (1) unit can be formed by polymerization of a formula (1) unit-forming monomer. The formula (1) unit-forming monomer is the following monomer (1M).
[0038]
[0039] In the monomer (1M), R 1 , R 2 , R 3 , X 1 , X 2 , —O—, —NH—, and m respectively represent R 1 , R 2 , R 3 , X 1 , X 2 , -O-, -NH-, and m. For specific examples of the monomer (1M), see the examples of the monomer for forming the unit of formula (1) in the Examples section below. The ratio (mass %) of the amount of the monomer (1M) charged to the amount of all the monomers charged when producing the polymer dispersant corresponds to the content (mass %) of the unit of formula (1) relative to the total amount of the polymer dispersant, as described above.
[0040] (Structural Unit Represented by Formula (2)) The polymer dispersant containing a crosslinked structure contains at least one unit of formula (2) (i.e., a structural unit represented by formula (2)).
[0041]
[0042] In formula (2), R 4 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; R5 represents an alkyl group having 8 or more carbon atoms; X 3 represents —O— or —NH—.
[0043] In formula (2), R 4 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 4 is preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, more preferably a hydrogen atom, a methyl group, or an ethyl group, and even more preferably a hydrogen atom or a methyl group.
[0044] In formula (2), R 5 represents an alkyl group having 8 or more carbon atoms. 5 is preferably an alkyl group having 8 to 50 carbon atoms, more preferably an alkyl group having 8 to 40 carbon atoms, even more preferably an alkyl group having 8 to 30 carbon atoms, even more preferably an alkyl group having 10 to 30 carbon atoms, and even more preferably an alkyl group having 12 to 25 carbon atoms.
[0045] In formula (2), X 3 represents —O— or —NH—. 3 is preferably —O—.
[0046] The content of the unit of formula (2) relative to the total amount of the polymer dispersant containing a crosslinked structure is preferably 3% by mass to 80% by mass, more preferably 5% by mass to 70% by mass, even more preferably 10% by mass to 60% by mass, and still more preferably 10% by mass to 50% by mass.
[0047] The content of the unit of formula (2) relative to the total amount of the polymer dispersant containing a crosslinked structure, excluding the crosslinked structure, is preferably 3% by mass to 80% by mass, more preferably 5% by mass to 70% by mass, even more preferably 10% by mass to 60% by mass, and still more preferably 10% by mass to 50% by mass.
[0048] The formula (2) unit can be formed by polymerization of a monomer for forming the formula (2) unit. The monomer for forming the formula (2) unit is the following monomer (2M).
[0049]
[0050] In the monomer (2M), R 4 , R 5 , and X3 are R in formula (2), respectively. 4 , R 5 , and X 3 For specific examples of the monomer (2M), see the examples of the monomer for forming the unit of formula (2) in the Examples section below. The ratio (mass %) of the amount of the monomer (2M) charged to the amount of all the monomers charged when producing the polymer dispersant corresponds to the content (mass %) of the unit of formula (2) relative to the total amount of the polymer dispersant, as described above.
[0051] (Crosslinked Structure) In the pigment dispersion of the present disclosure, the polymeric dispersant containing a crosslinked structure can be formed by crosslinking an uncrosslinked polymeric dispersant (i.e., a polymeric dispersant that does not contain a crosslinked structure before crosslinking). The polymeric dispersant containing a crosslinked structure is preferably a reaction product of an uncrosslinked polymeric dispersant containing an acid group (e.g., a carboxy group) and a crosslinking agent. In this case, the crosslinked structure is a structure formed by a reaction (e.g., an acid-epoxy reaction) between the acid group and a crosslinkable group in the crosslinking agent (e.g., an epoxy group in an epoxy compound).
[0052] In the present disclosure, the term "acid group" encompasses both an unneutralized acid group (e.g., a carboxy group) and a neutralized acid group (e.g., a salt of a carboxy group (e.g., -C(=O)ONa)). Neutralization will be described later.
[0053] The pigment dispersion of the present disclosure can be preferably produced by dispersing a pigment using an uncrosslinked polymeric dispersant containing acid groups to produce a dispersion (hereinafter referred to as the "uncrosslinked dispersion"), mixing the resulting uncrosslinked dispersion with a crosslinking agent, and reacting the acid groups in the uncrosslinked polymeric dispersant in the uncrosslinked dispersion with the crosslinking agent. This reaction causes the acid groups in the uncrosslinked polymeric dispersant to react with the crosslinking agent, forming a crosslinked structure. This crosslinked structure formation reaction is thought to proceed in a state in which the uncrosslinked polymeric dispersant is adsorbed on the pigment surface. Therefore, the formation of the crosslinked structure is thought to have the effect of making it difficult for the polymeric dispersant to detach from the pigment surface.
[0054] Crosslinking Agent: A preferred crosslinking agent is a compound having two or more reactive sites with an uncrosslinked polymeric dispersant (e.g., an uncrosslinked polymeric dispersant containing a carboxy group). A preferred combination of a crosslinking agent and an uncrosslinked polymeric dispersant is a combination of a compound having two or more epoxy groups (i.e., a bifunctional or higher epoxy compound) as the crosslinking agent and an uncrosslinked polymeric dispersant containing at least one of a carboxy group and a salt thereof as the uncrosslinked polymeric dispersant. In this combination, a crosslinked structure is formed by reaction between at least one of a carboxy group and a salt thereof in the uncrosslinked polymeric dispersant containing at least one of a carboxy group and a salt thereof and an epoxy group in the compound containing two or more epoxy groups, thereby forming a polymeric dispersant containing a crosslinked structure. The formation of such a crosslinked structure is preferably carried out after dispersing the pigment with an uncrosslinked polymeric dispersant containing at least one of a carboxy group and a salt thereof.
[0055] Specific examples of difunctional or higher functional epoxy compounds, which are preferred embodiments of the crosslinking agent, include ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, diethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, dipropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, trimethylolpropane triglycidyl ether, etc. Among these, polyethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, and trimethylolpropane triglycidyl ether are preferred.
[0056] Commercially available crosslinking agents may also be used, such as Denacol EX-321, EX-821, EX-830, EX-850, and EX-851 (manufactured by Nagase ChemteX Corporation).
[0057] The molar ratio of the crosslinking moiety (e.g., epoxy group) in the crosslinking agent to the crosslinkable moiety (e.g., carboxy group or a salt thereof) in the uncrosslinked polymer dispersant [crosslinking moiety (e.g., epoxy group) in the crosslinking agent:crosslinkable moiety (e.g., carboxy group or a salt thereof) in the uncrosslinked polymer dispersant] is preferably 1:1.1 to 1:10, more preferably 1:1.1 to 1:5, and even more preferably 1:1.1 to 1:3, from the viewpoint of the crosslinking reaction rate and / or the stability of the dispersion after crosslinking.
[0058] (Uncrosslinked Polymeric Dispersant) An uncrosslinked polymeric dispersant (i.e., a polymeric dispersant before a crosslinked structure is formed) can also contain units of formula (1) and units of formula (2), similar to polymeric dispersants containing a crosslinked structure. The units of formula (1) and formula (2) are not changed by the reaction to form a crosslinked structure, and can be maintained as they are in a polymeric dispersant containing a crosslinked structure.
[0059] The preferred range of the content of the formula (1) unit relative to the total amount of the uncrosslinked polymeric dispersant is the same as the preferred range of the content of the formula (1) unit relative to the total amount of the polymeric dispersant containing a crosslinked structure, excluding the crosslinked structure. The preferred range of the content of the formula (2) unit relative to the total amount of the uncrosslinked polymeric dispersant is the same as the preferred range of the content of the formula (2) unit relative to the total amount of the polymeric dispersant containing a crosslinked structure, excluding the crosslinked structure.
[0060] The uncrosslinked polymeric dispersant may further contain acid groups. A crosslinked structure is formed by the reaction of these acid groups with a crosslinking agent (e.g., an acid-epoxy reaction). A portion of the total number of acid groups in the uncrosslinked polymeric dispersant may remain in the polymeric dispersant containing a crosslinked structure.
[0061] As described above, the acid group contained in the uncrosslinked polymer dispersant may be a neutralized acid group or an unneutralized acid group. The neutralized acid group is preferably a -C(=O)OM group (where M represents an alkali metal, an ammonium ion, or an organic cation). Examples of the organic cation include alkylammonium cations having 1 to 10 carbon atoms, hydroxy-substituted alkylammonium cations having 1 to 10 carbon atoms, carboxy-substituted alkylammonium cations having 2 to 10 carbon atoms, and organic cations having 2 to 10 alkyleneimine units having 2 to 4 carbon atoms. The unneutralized acid group is preferably a carboxy group (-C(=O)OH group).
[0062] The acid groups can be neutralized by reacting the uncrosslinked polymer dispersant containing acid groups with a base (hereinafter also referred to as a "neutralizing base"). Examples of the neutralizing base include alkali metal hydroxides such as sodium hydroxide and potassium hydroxide; ammonia; and organic amines such as dimethylethanolamine and diisopropylethylamine.
[0063] Neutralization Rate: In an uncrosslinked polymeric dispersant, it is preferable that 10% to 90% of the total number of acid groups contained therein are neutralized (i.e., salts of acid groups). In other words, in an uncrosslinked polymeric dispersant, the proportion of neutralized acid groups to the total number of neutralized and unneutralized acid groups (i.e., % by number; hereinafter, also referred to as "neutralization rate (%)") is preferably 10% to 90%. When the neutralization rate (%) is 10% to 90%, a crosslinked structure is more likely to be formed. The neutralization rate (%) is preferably 20% to 80%, more preferably 20% to 60%. The neutralization rate (%) is determined by neutralization titration.
[0064] - Acid group unit - Both the uncrosslinked polymeric dispersant and the polymeric dispersant containing a crosslinked structure preferably contain a structural unit derived from a monomer containing an acid group (hereinafter also referred to as an "acid group unit"). Here, a structural unit derived from a monomer containing an acid group means a structural unit formed using a monomer containing an acid group as a raw material. In the structural unit derived from the monomer containing an acid group (i.e., acid group unit), the acid group may remain as it is, or may have disappeared. For example, after a structural unit is formed by polymerization of a monomer containing an acid group, the acid group in this structural unit may have disappeared due to a crosslinked structure-forming reaction.
[0065] The monomer containing an acid group is preferably a compound containing an acid group and a polymerizable group. The polymerizable group is more preferably a group containing an ethylenic double bond, and further preferably a (meth)acryloyl group, an allyl group, a styryl group, or a vinyl group.
[0066] Specific examples of the monomer containing an acid group include (meth)acrylic acid, β-carboxyethyl acrylate, fumaric acid, itaconic acid, maleic acid, crotonic acid, etc. Among these, (meth)acrylic acid is particularly preferred.
[0067] The content of the acid group units relative to the total amount of the uncrosslinked polymeric dispersant or the polymeric dispersant containing a crosslinked structure is preferably 10% by mass to 70% by mass, more preferably 15% by mass to 65% by mass, and even more preferably 20% by mass to 60% by mass.
[0068] —Hydrophilic / Hydrophobic Ratio— When the polymer dispersant containing a crosslinked structure contains a unit of formula (1), a unit of formula (2), and an acid group unit, the hydrophilic / hydrophobic ratio represented by the following formula is preferably equal to or greater than 8. This further improves the stability over time of the pigment dispersion.
[0069] Hydrophilic / hydrophobic ratio = (mass ratio of the units of formula (2) to the total mass of the polymer dispersant containing a crosslinked structure × R in formula (2)) 2 (number of carbon atoms in the alkylene group represented by the formula (I)) / (mass ratio of acid group units to the total mass of the polymer dispersant including the crosslinked structure)
[0070] From the viewpoint of further improving the stability over time of the pigment dispersion and from the viewpoint of ensuring the affinity of the polymer dispersant containing a crosslinked structure for water, the hydrophilic / hydrophobic ratio is preferably 8 or more and 60 or less, more preferably 10 or more and 50 or less, and even more preferably 12 or more and 40 or less.
[0071] —Ar Valence— In a crosslinked polymer dispersant containing a crosslinked structure, the Ar valence represented by the following formula is preferably 0.3 mmol / g to 3.1 mmol / g, and more preferably 0.4 mmol / g to 2.9 mmol / g, from the viewpoint of further improving the stability over time of the pigment dispersion.
[0072] Ar valence = (number of mmoles of formula (1) units per 1 g of polymer dispersant containing a crosslinked structure) × (number of aromatic rings in formula (1) units)
[0073] Here, the number of aromatic rings in the unit of formula (1) is n for n-fused rings (where n is an integer of 2 or more).
[0074] -Other structural units- Each of the uncrosslinked polymeric dispersant and the polymeric dispersant containing a crosslinked structure may contain structural units other than the formula (1) unit, the formula (2) unit, and the acid group unit (hereinafter also referred to as "other structural units"). However, the total proportion of the formula (1) unit, the formula (2) unit, and the acid group unit in the total amount of the uncrosslinked polymeric dispersant or the polymeric dispersant containing a crosslinked structure is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more.
[0075] Examples of the other structural units include structural units derived from vinyl monomers. Examples of the vinyl monomer include methyl (meth)acrylate. The other structural units in the uncrosslinked polymer dispersant may remain in the polymer dispersant containing a crosslinked structure.
[0076] -Weight-average molecular weight (Mw) of uncrosslinked polymer dispersant- The weight-average molecular weight (Mw) of the uncrosslinked polymer dispersant is not particularly limited, but from the viewpoint of pigment dispersibility, it is preferably 3,000 to 200,000, more preferably 5,000 to 150,000, and even more preferably 10,000 to 100,000.
[0077] In the present disclosure, the weight average molecular weight (Mw) is measured by gel permeation chromatography (GPC). GPC is performed using an HLC-8220GPC (manufactured by Tosoh Corporation), with three columns connected in series: TSKgeL SuperHZM-H, TSKgeL SuperHZ4000, and TSKgel SuperHZ2000 (all trade names manufactured by Tosoh Corporation), and THF (tetrahydrofuran) as the eluent. The conditions are a sample concentration of 0.45% by mass, a flow rate of 0.35 ml / min, a sample injection amount of 10 μl, and a measurement temperature of 40°C, and the measurement is performed using a differential refractive index detector. In addition, a calibration curve is prepared from eight samples of "Standard Sample TSK Standard, Polystyrene" manufactured by Tosoh Corporation: "F-40", "F-20", "F-4", "F-1", "A-5000", "A-2500", "A-1000", and "n-propylbenzene".
[0078] In the pigment dispersion of the present disclosure, the ratio of the content of the pigment to the content of the polymer dispersant having a crosslinked structure, on a mass basis, is preferably 1:0.04 to 1:3, more preferably 1:0.05 to 1:1, and even more preferably 1:0.05 to 1:0.5.
[0079] In the uncrosslinked dispersion, the ratio of the pigment content to the uncrosslinked polymer dispersant content, on a mass basis, is preferably 1:0.04 to 1:3, more preferably 1:0.05 to 1:1, and even more preferably 1:0.05 to 1:0.5.
[0080] The uncrosslinked polymeric dispersant can be produced by a known method of copolymerizing each monomer for forming each structural unit (i.e., a monomer for forming a unit of formula (1), a monomer for forming a unit of formula (2), a monomer containing an acid group, etc.).
[0081] <Other Components> The pigment dispersion of the present disclosure may contain other components in addition to the components described above. Examples of the other components include components that can be contained in an ink composition. Examples of the other components include a water-soluble organic solvent.
[0082] In the present disclosure, "water-soluble" means the property of dissolving 1 g or more in 100 g of water at 25°C.
[0083] Specific examples of water-soluble organic solvents are as follows: Alcohols (e.g., methanol, ethanol, propanol, isopropanol, butanol, isobutanol, secondary butanol, tertiary butanol, pentanol, hexanol, cyclohexanol, benzyl alcohol, etc.), Polyhydric alcohols (e.g., ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, propylene glycol, dipropylene glycol, polypropylene glycol, butylene glycol, hexanediol, pentanediol, glycerin, hexanetriol, thiodiglycol, 2-methylpropanediol, etc.). Polyhydric alcohol ethers (for example, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monobutyl ether, tripropylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol dimethyl ether, ethylene glycol monomethyl ether acetate, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, triethylene glycol monobutyl ether, ethylene glycol monophenyl ether, propylene glycol monophenyl ether, etc.).
[0084] The total amount of water, pigment, and polymer dispersant having a crosslinked structure in the total amount of the pigment dispersion of the present disclosure is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more.
[0085] <Example of Pigment Dispersion Manufacturing Method (Manufacturing Method A)> An example of a method for manufacturing a pigment dispersion of the present disclosure (hereinafter referred to as Manufacturing Method A) is shown below. Manufacturing Method A includes the steps of: manufacturing an acid group-containing polymer containing units of Formula (1), units of Formula (2), and acid groups; neutralizing at least a portion of the total number of acid groups in the manufactured acid group-containing polymer with a base to obtain an uncrosslinked polymeric dispersant; dispersing a pigment in water with the uncrosslinked polymeric dispersant to obtain an uncrosslinked dispersion containing water, the pigment, and the uncrosslinked polymeric dispersant; and reacting the uncrosslinked polymeric dispersant in the uncrosslinked dispersion with a crosslinking agent to obtain a pigment dispersion containing water, the pigment, and a polymeric dispersant containing a crosslinked structure.
[0086] The neutralization of the acid group-containing polymer to obtain the uncrosslinked polymeric dispersant and its preferred embodiments are as described above. The step of obtaining the uncrosslinked dispersion can be carried out using a conventional pigment dispersion technique. Examples of dispersing machines used for pigment dispersion include a ball mill, a roll mill, a sand mill, a bead mill, and a Nanomizer. The reaction between the uncrosslinked polymeric dispersant and the crosslinking agent (i.e., the formation of a crosslinked structure) in the step of obtaining the pigment dispersion and its preferred embodiments are as described above.
[0087] [Ink Composition] The ink composition of the present disclosure contains the pigment dispersion of the present disclosure described above. That is, the ink composition of the present disclosure contains the components of the pigment dispersion of the present disclosure described above. The ink composition of the present disclosure can be produced by adding any component to the pigment dispersion of the present disclosure described above. Alternatively, the ink composition of the present disclosure may be the pigment dispersion of the present disclosure itself. That is, the ink composition of the present disclosure may satisfy the requirements of the pigment dispersion of the present disclosure described above.
[0088] The ink composition of the present disclosure is preferably an inkjet ink. In this case, the inkjet recording method can be appropriately described by reference to the descriptions in known documents.
[0089] <Water> The ink composition of the present disclosure contains water. The water content relative to the total amount of the ink composition is preferably 30% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, and still more preferably 60% by mass or more. The upper limit of the water content relative to the total amount of the ink composition is, for example, 90% by mass or 80% by mass.
[0090] <Pigment> The ink composition of the present disclosure contains at least one pigment. Preferred embodiments of the pigment are as described in the "Pigment Dispersion" section. The content of the pigment relative to the total amount of the ink composition is preferably 1% by mass to 30% by mass, more preferably 1.5% by mass to 20% by mass, even more preferably 2% by mass to 15% by mass, and even more preferably 2% by mass to 10% by mass.
[0091] <Polymer dispersant containing a crosslinked structure> The ink composition of the present disclosure contains at least one polymer dispersant containing a crosslinked structure. Preferred embodiments of the polymer dispersant containing a crosslinked structure are as described in the section "Pigment dispersion."
[0092] The ratio of the content of the pigment to the content of the polymer dispersant having a crosslinked structure is preferably from 1:0.04 to 1:3, more preferably from 1:0.05 to 1:1, and even more preferably from 1:0.05 to 1:0.5, on a mass basis.
[0093] <Water-soluble organic solvent> The ink composition of the present disclosure preferably contains a water-soluble organic solvent. This improves the ejection properties from an inkjet head when the ink composition of the present disclosure is used as an inkjet ink. Specific examples of the water-soluble organic solvent are as shown in the section "Pigment dispersion." The content of the water-soluble organic solvent relative to the total amount of the ink composition is preferably 5% by mass to 40% by mass, more preferably 10% by mass to 30% by mass, and even more preferably 15% by mass to 30% by mass.
[0094] <Urea> The ink composition of the present disclosure preferably contains urea. Urea functions as a solid humectant. The content of urea relative to the total amount of the ink composition is preferably 1% by mass to 10% by mass, more preferably 2% by mass to 9% by mass, and even more preferably 3% by mass to 8% by mass.
[0095] <Other Components> The ink composition of the present disclosure may contain other components as necessary. Examples of other components include additives such as surfactants, resin particles, water-soluble resins, silicon compounds, UV absorbers, antioxidants, anti-fading agents, conductive salts, and basic compounds (pH adjusters). For information on components that can be contained in the ink composition, reference can be made to known documents such as JP-A-2015-193729 and JP-A-2016-069487.
[0096] <Physical Properties> The pH (25°C) of the ink composition is preferably 7 to 10, and more preferably 7.5 to 9.5. The pH is measured at 25°C using a pH meter, for example, a pH meter manufactured by Toa DKK Corporation (model number "HM-31")
[0097] The viscosity (30°C) of the ink composition is preferably 0.5 mPa·s to 30 mPa·s, more preferably 2 mPa·s to 20 mPa·s, even more preferably 2 mPa·s to 15 mPa·s, and even more preferably 3 mPa·s to 10 mPa·s. The viscosity is a value measured at 25°C using a viscometer. The viscosity is measured at 25°C using a viscometer, for example, a TV-22 viscometer manufactured by Toki Sangyo Co., Ltd.
[0098] The surface tension (25°C) of the ink composition is preferably 60 mN / m or less, more preferably 20 mN / m to 50 mN / m, and even more preferably 30 mN / m to 45 mN / m. The surface tension is measured at 25°C using a surface tensiometer, for example, an automatic surface tensiometer (product name "CBVP-Z" manufactured by Kyowa Interface Science Co., Ltd.) by the plate method.
[0099] The present disclosure will be described in more detail below with reference to examples, but the present disclosure is not limited to the following examples as long as it does not depart from the gist of the disclosure. Hereinafter, the polymer dispersant may be simply referred to as a "dispersant."
[0100] <Synthesis of Uncrosslinked Dispersants> Dispersants A1 to A28 and comparative dispersants C1 to C3 shown in Table 1 were synthesized as uncrosslinked dispersants.
[0101] (Synthesis of Dispersant A1) A reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer was charged with 153.5 parts by mass of tripropylene glycol monomethyl ether (product name "MFTG", manufactured by Nippon Nyukazai Co., Ltd.) as a reaction solvent, and then the atmosphere inside the reaction vessel was replaced with nitrogen gas. Next, the reaction vessel was heated to 85°C, and the following were added: 76.8 parts by mass of MFTG as a reaction solvent, nonylphenoxypentapropylene glycol acrylate (NPh(PO)) as a monomer for forming units of formula (1), 5 A mixture of 16 parts by weight of stearyl methacrylate (STMA) as a monomer for forming units of Formula (2), 54 parts by weight of methacrylic acid (MAA) as a monomer for forming acid group-containing units, 2 parts by weight of methyl methacrylate (MMA) as an additional monomer, and 3 parts by weight of V-601 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as a polymerization initiator was added dropwise over 3 hours to carry out a polymerization reaction. After completion of the addition, the mixture was allowed to react for another 4 hours at 85 ° C to obtain a solution containing a polymer. The resulting solution was cooled to room temperature, and then 251 parts by weight of a 1 mol / L NaOH aqueous solution was added as an aqueous solution of a neutralizing base to neutralize 40% of the total number of carboxy groups in the polymer (i.e., neutralization at a neutralization rate of 40%). Water was added to the neutralized solution so that the dispersant A1 concentration was 5.6% by weight, obtaining a solution of dispersant A1.
[0102] Table 1 shows the type and amount (parts by mass) of monomers used to form the uncrosslinked dispersant, the neutralizing base used to neutralize the carboxyl groups in the uncrosslinked dispersant, the neutralization rate (%) of the carboxyl groups in the uncrosslinked dispersant, the weight average molecular weight (Mw) of the uncrosslinked dispersant, the hydrophilic / hydrophobic ratio of the crosslinked dispersant, and the Ar value (mmol / g) of the crosslinked dispersant. The methods for measuring Mw, calculating the hydrophilic / hydrophobic ratio, and calculating the Ar value are as described above. In the classification of monomers in Table 1, "Formula (1)," "Formula (2)," "Acid group," and "Other" refer to the Formula (1) unit-forming monomer, the Formula (2) unit-forming monomer, the acid group-containing unit-forming monomer, and other monomers, respectively.
[0103] (Synthesis of Dispersants A2 to A28, Comparative Dispersants C1 to C3) Dispersants A2 to A28 and Comparative Dispersants C1 to C3 were synthesized as uncrosslinked dispersants in the same manner as in the synthesis of Dispersant A1, except that the monomer composition (type and amount charged) and neutralization base were changed as shown in Table 1 below.
[0104] Example 1 Preparation of Uncrosslinked Dispersion A mixture of the following composition was pre-dispersed to a uniform consistency, and then dispersed for 3 hours using a beads mill (bead diameter: 0.1 mm, zirconia beads), to obtain an uncrosslinked dispersion in which the magenta pigment was dispersed using Dispersant A1.
[0105] - Composition of uncrosslinked dispersion - Pigment Red 122 (magenta pigment) ... 20.4 parts by mass Solution of dispersant A1 (uncrosslinked dispersant) ... 35.8 parts by mass MFTG ... 6.1 parts by mass Water ... 73.7 parts by mass
[0106] <Production of Crosslinked Dispersion> Next, a mixture having the following composition was reacted at 70°C for 6 hours and then cooled to 25°C. Dispersant A1 (uncrosslinked polymer dispersant) in the uncrosslinked dispersion was crosslinked with the crosslinking agent, thereby obtaining a crosslinked dispersion containing water, a pigment, and a polymer dispersant having a crosslinked structure (hereinafter also referred to as "crosslinked dispersant").
[0107] - Composition - Uncrosslinked dispersion... 136.0 parts by mass "Denacol EX-321" (manufactured by Nagase ChemteX Corporation) (trimethylolpropane polyglycidyl ether; crosslinking agent)... 3.0 parts by mass
[0108] <Production of Pigment Dispersion as Target Product> Next, the crosslinked dispersion was ultrafiltered by passing it through an ultrafiltration device (crossflow ultrafilter (UF), manufactured by Sartorius) equipped with a polyethersulfone (PESU) membrane (micropore size: 0.1 μm) at a flow rate of 600 mL per minute. The liquid temperature was adjusted to 25°C, and ultrafiltration was performed 10 times, with one run being equal to the volumetric expansion of the charged liquid. Thereafter, ion-exchanged water was added so that the pigment concentration was 15% by mass. In this manner, a pigment dispersion as the target product (hereinafter referred to as "pigment dispersion A") containing water, the pigment, and a crosslinked dispersant (i.e., a polymer dispersant having a crosslinked structure) was obtained.
[0109] <Preparation of Ink Composition> A mixture of the following components was stirred and mixed to a uniform consistency to obtain an ink composition: The ink composition below contains 5 parts by mass of pigment and 1.5 parts by mass of dispersant.
[0110] - Composition of ink composition - Pigment dispersion A: 33.3 parts by mass; Propylene glycol (water-soluble organic solvent): 20.0 parts by mass; Hexyl glycol (water-soluble organic solvent): 3.4 parts by mass; Urea: 5.0 parts by mass; Water: 38.3 parts by mass
[0111] <Evaluation of temporal stability of ink composition> The ink composition (30 mL) was filled into a sample bottle and sealed. Hereinafter, this ink composition will be referred to as "ink before storage". Next, the ink before heating was heated to 80°C and stored at 80°C for 24 hours. Hereinafter, the ink after being left at 80°C for 24 hours will be referred to as "ink after storage". The average particle size of each of the ink before storage and the ink after storage was measured using a Nanotrac wave II (manufactured by Microtrackbell Co., Ltd.), and the particle size change rate was calculated according to the following formula.
[0112] Particle size change rate (%) = [((average particle size in ink after storage) - (average particle size in ink before storage)) / (average particle size in ink before storage)] x 100
[0113] Based on the obtained rate of change in particle diameter, the temporal stability of the ink composition was determined according to the following evaluation criteria: In the following evaluation criteria, the ink composition with the most excellent temporal stability is ranked "A."
[0114] - Evaluation criteria for stability over time - A: Particle size change rate is less than 10% B: Particle size change rate is 10% or more but less than 25% C: Particle size change rate is 25% or more but less than 50% D: Particle size change rate is 50% or more
[0115] [Examples 2 to 30, Comparative Examples 1 to 3] The same procedure as in Example 1 was carried out, except that the type of uncrosslinked dispersant and the type of pigment were changed as shown in Table 1. The results are shown in Table 1.
[0116]
[0117] For the pigments in Table 1, PR122, PY150, and PB15:3 refer to Pigment Red 122, Pigment Yellow 150, and Pigment Blue 15:3, respectively.
[0118] The abbreviations and structures of the monomers in Table 1 are as follows: NPh(PO) 5 A: Nonylphenoxypentapropylene glycol acrylate NPh(EO) 8 A: Nonylphenoxyoctaethylene glycol acrylate OPhPh(EO) 2 A: Orthophenylphenoxyethylene glycol acrylate Ph(EO) 2 A: Phenoxydiethylene glycol acrylate Npt(EO) 2 A: Naphthoxydiethylene glycol methacrylate Fu(EO) 2 A: Furyl diethylene glycol acrylate Ph(EO) 4 A: Phenoxytetraethylene glycol acrylate NPh(EO) 4A: Nonylphenoxytetraethylene glycol acrylate PhEMA: Phenoxyethyl methacrylate BzMA: Benzyl methacrylate STMA: Stearyl methacrylate LMA: Lauryl methacrylate VA: Behenyl acrylate HA: Hexyl acrylate MAA: Methacrylic acid AA: Acrylic acid MMA: Methyl methacrylate
[0119]
[0120] For the neutralizing bases in Table 1, DMEA means dimethylethanolamine and DIPEA means diisopropylethylamine.
[0121] As shown in Table 1, the inks in all Examples had good stability over time. In all Examples, the cross-linked dispersant in the pigment dispersion was a compound represented by the formula (1) where m is an integer of 2 or more and R 5 The dispersant used was an alkyl group having 8 or more carbon atoms.
[0122] The results of the comparative examples compared to the examples were as follows. Comparative Example 1 is a comparative example in which m in formula (1) was changed to 1 (specifically, the formula (1) unit was changed to a PhEMA unit). Comparative Example 2 is a comparative example in which m in formula (1) was changed to 0 (specifically, the formula (1) unit was changed to a BzMA unit). Comparative Example 3 is a comparative example in which R 5 These are comparative examples in which the number of carbon atoms in the alkyl group represented by the formula (2) was changed to 6 (more specifically, the formula (2) unit was changed to an HA unit). In all of Comparative Examples 1 to 3, the ink stability over time was reduced.
[0123] The disclosure of Japanese Patent Application No. 2023-059325, filed on March 31, 2023, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.
Claims
1. A pigment dispersion comprising water, a pigment, and a polymer dispersant having a crosslinked structure, the polymer dispersant having a crosslinked structure further comprising a structural unit represented by the following formula (1) and a structural unit represented by the following formula (2). In formula (1), R 1 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; R 2 represents an alkylene group having 2 to 5 carbon atoms; R 3 represents an aromatic group; 1 and X 2 each independently represents -O- or -NH-, and m represents an integer of 2 or more. 4 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; R 5 represents an alkyl group having 8 or more carbon atoms; 3 represents --O-- or --NH--.
2. The pigment dispersion according to claim 1, wherein the polymer dispersant containing a crosslinked structure further contains a structural unit derived from a monomer containing an acid group, and the hydrophilic / hydrophobic ratio represented by the following formula is 8 or more. Hydrophilic / hydrophobic ratio = (mass ratio of the structural unit represented by formula (2) to the total mass of the polymer dispersant containing a crosslinked structure × the R in formula (2) 2 (the number of carbon atoms in the alkylene group represented by the formula (I)) / (the mass ratio of the structural unit derived from the monomer containing an acid group to the total mass of the polymer dispersant containing a crosslinked structure) 3. The pigment dispersion according to claim 1, wherein the polymer dispersant containing a crosslinked structure has an Ar valence, represented by the following formula, of 0.4 mmol / g to 2.9 mmol / g: Ar valence = (number of mmoles of the structural unit represented by formula (1) per gram of the polymer dispersant containing a crosslinked structure) x (number of aromatic rings in the structural unit represented by formula (1)).
4. In the formula (1), 2 The pigment dispersion according to claim 1 , wherein R represents an alkylene group having 2 carbon atoms.
5. The pigment dispersion according to claim 1, wherein the polymeric dispersant containing a crosslinked structure is formed by crosslinking an uncrosslinked polymeric dispersant, and the uncrosslinked polymeric dispersant contains a structural unit represented by formula (1), a structural unit represented by formula (2), and an acid group, and 10% to 90% of the total number of the acid groups contained therein are neutralized.
6. An ink composition comprising the pigment dispersion according to any one of claims 1 to 5.
Citation Information
Patent Citations
Photopolymerization composition, photopolymerizable color composition and color filter
JP2002012607A
Actinic energy ray-curable ink-jet ink
JP2002188025A
Recording liquid
JP2003026978A
Black ink for ink-jet recording and method for forming image