(METH)acrylate-modified phenol resin, curable composition, cured product, prepreg, circuit board, build-up film, semiconductor sealing material and semiconductor device

The (meth)acrylate-modified phenolic resin addresses the need for low dielectric loss tangent and thermal expansion in electronic components by modifying the phenolic resin with a fluorene structural unit, resulting in cured products with improved performance for electronic applications.

JP2024159338APending Publication Date: 2024-11-08DIC CORP
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
JP2023075274
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing resin compositions, such as modified polyphenylene ethers, fail to adequately meet the requirements of low dielectric loss tangent and low coefficient of thermal expansion needed for advanced electronic components as they become smaller and thinner.

Method used

A (meth)acrylate-modified phenolic resin is developed by modifying the hydroxyl group of a phenolic resin with a fluorene structural unit at the 9-position, incorporating a (meth)acrylate group to achieve both low dielectric loss tangent and low coefficient of thermal expansion.

Benefits of technology

The (meth)acrylate-modified phenolic resin provides cured products with both low dielectric loss tangent and low coefficient of thermal expansion, suitable for use in prepregs, circuit boards, build-up films, semiconductor encapsulants, and semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159338000051
    Figure 2024159338000051
  • Figure 2024159338000052
    Figure 2024159338000052
  • Figure 2024159338000053
    Figure 2024159338000053
Patent Text Reader

Abstract

To provide a (meth)acrylate-modified phenol resin which has low dielectric loss tangent and low thermal expansion coefficient and enables the low dielectric loss tangent and the low thermal expansion coefficient to be made highly compatible with each other.SOLUTION: A (meth)acrylate-modified phenol resin is provided, which is a (meth)acrylic ester of a reaction product of a fluorene compound (having no substituent at 9-position), a phenolic hydroxyl group-containing compound and a compound represented by general formula (1). In the formula, Ar is Ar1-Y-Ar1 or Ar1, Ar1 is each independently an aromatic cyclic group that may have a substituent, Y is a single bond, an aliphatic hydrocarbon group having 1 to 6 carbon numbers, -P(=O)Ra- group, an oxygen atom, a sulfur atom or a sulfonyl group, Ra is an aromatic cyclic group, R1 is each independently a hydrogen atom or an aliphatic hydrocarbon group having 1 to 4 carbon atoms, and X is a desorption group.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a (meth)acrylate-modified phenolic resin, a curable composition, a cured product, a prepreg, a circuit board, a build-up film, a semiconductor encapsulant, and a semiconductor device. [Background technology]

[0002] Epoxy resin compositions containing an epoxy resin and a curing agent therefor exhibit excellent heat resistance and insulating properties in the cured product, and are therefore widely used in electronic component applications such as semiconductors and multilayer printed circuit boards. Among these electronic component applications, in the technical field of sealing materials and circuit board materials, there is a demand for resin compositions that, when cured, exhibit a sufficiently low dielectric tangent, in response to the recent trend toward faster and higher-frequency signals in various electronic devices. In addition, there is a demand for materials with a reduced thermal expansion coefficient as a countermeasure against warpage associated with the miniaturization and thinning of circuit boards. In response to this, modified polyphenylene ethers have been proposed in order to improve the dielectric properties (particularly low dielectric tangent) and low thermal expansion coefficient in the high frequency range (for example, Non-Patent Documents 1 and 2). [Prior art documents] [Non-patent literature]

[0003] [Non-Patent Document 1] Shoya Sekiguchi, "Application of polyphenylene ether to low-loss materials," Journal of Network Polymers Vol. 44 No. 1 P35-40(2023) [Non-Patent Document 2] Shin Takanezawa and 9 others, "Development of Ultra-Low Thermal Expansion Board Materials for Semiconductor Packaging," Journal of the Japan Institute of Electronics Packaging Vol. 19 No. 6 P421-426 (2016) Summary of the Invention [Problem to be solved by the invention]

[0004] However, the above-mentioned modified polyphenylene ethers do not fully satisfy the properties required in recent years, and there is still a demand for resins that can simultaneously achieve a higher level of low dielectric tangent and low thermal expansion coefficient. [Means for solving the problem]

[0005] As a result of intensive research aimed at solving the above-mentioned problems, the inventors have discovered that a resin in which the hydroxyl group of a phenolic resin having a structure in which the hydrogen atom at the 9th position of a fluorene structural unit is modified with an aralkyl is modified with a (meth)acrylate, thereby achieving both a low dielectric tangent and a low thermal expansion coefficient to a high degree, and have thus completed the present invention.

[0006] The gist of the present invention is as follows. [1] A (meth)acrylate-modified phenolic resin which is a (meth)acrylate ester of a reaction product of a fluorene compound (having no substituent at the 9-position), a phenolic hydroxyl group-containing compound, and a compound represented by general formula (1): [ka] (where: Ar is Ar 1 -Y-Ar 1 Or Ar 1 and Ar 1 each independently represents an aromatic ring group which may have a substituent, Y is a single bond, an aliphatic hydrocarbon group having 1 to 6 carbon atoms, -P(=O)R a - group, oxygen atom, sulfur atom or sulfonyl group, R a is an aromatic ring group, R 1 each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 4 carbon atoms, X is a leaving group. [2] The (meth)acrylate-modified phenolic resin according to [1], wherein the amount of the fluorene compound is 0.01 to 0.99 mol per 1 mol of the compound represented by the general formula (1). [3] A (meth)acrylate-modified phenolic resin represented by general formula (15): [ka] (where: Z is independently a group represented by the general formula (12A): [ka] or a structural unit represented by general formula (13A): [ka] It is a structural unit represented by Z' is independently a group represented by the general formula (12A'): [ka] or a structural unit represented by general formula (13A'): [ka] It is a structural unit represented by Ar is independently Ar 1 Or Ar 1 -Y-Ar 1 and Ar 1 each independently represents an aromatic ring group which may have a substituent, Y is a single bond, an aliphatic hydrocarbon group having 1 to 6 carbon atoms, -P(=O)R a - group, oxygen atom, sulfur atom or sulfonyl group, R a is an aromatic ring group, R 1 each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 4 carbon atoms, R 2 each independently represents an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, m is independently an integer of 0 to 4, R b are each independently a hydrogen atom or a methyl group, R 3 are each independently an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, or two R 3 may form a ring together with the carbon atom to which they are attached, n is independently an integer of 0 to 3, R 2’ each independently represents an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, m' is independently an integer of 0 to 4, R b’ are each independently a hydrogen atom or a methyl group, R 3’ are each independently an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, or two R 3’ may form a ring together with the carbon atom to which they are attached, Each n' is independently an integer of 0 to 4, p is the average value and is a number greater than 0; however, The resin contains a structural unit represented by general formula (12A) and / or general formula (12A') and a structural unit represented by general formula (13A) and / or general formula (13A'). [4] The (meth)acrylate-modified phenolic resin according to [3], which contains at least one of a compound represented by general formula (15-1) and a compound represented by general formula (15-2). [ka] (where: Ar, Z, R 1 , R b’ , R 3’ and n' are as defined in [3].) [5] The (meth)acrylate-modified phenolic resin according to any one of [1] to [4], having a vinyl equivalent of 100 to 10,000. [6] The (meth)acrylate-modified phenolic resin according to any one of [1] to [5], having a number average molecular weight of 100 to 10,000. [7] A curable composition containing the (meth)acrylate-modified phenolic resin according to any one of [1] to [6]. [8] A cured product of the curable composition of [7]. [9] A prepreg having a reinforcing substrate and a semi-cured product of the curable composition [7] impregnated into the reinforcing substrate.

[10] [9] A circuit board that is a laminate of prepreg and copper foil.

[11] A build-up film containing the curable composition of [7].

[12] A semiconductor encapsulant comprising the curable composition according to [7].

[13] A semiconductor device comprising the cured semiconductor encapsulant according to

[12] . Effect of the Invention

[0007] According to the present invention, it is possible to provide a (meth)acrylate-modified phenolic resin capable of achieving both a low dielectric tangent and a low thermal expansion coefficient at a high level, and also to provide a curable composition containing the (meth)acrylate-modified phenolic resin and a cured product thereof. Furthermore, by using the curable composition or the cured product thereof, it is possible to provide a prepreg, a circuit board, a build-up film, a semiconductor encapsulant, and a semiconductor device that achieve both a low dielectric tangent and a low thermal expansion coefficient at a high level. [Brief description of the drawings]

[0008] [Figure 1] 1 shows the results of GPC measurement of phenol resin A-1 synthesized in Example 1. [Diagram 2] 1 shows the results of 13C-NMR measurement of phenol resin A-1 synthesized in Example 1. [Diagram 3] 1 shows the results of FD-MS measurement of phenolic resin A-1 synthesized in Example 1. [Figure 4] 1 shows the results of GPC measurement of the methacrylate-modified phenolic resin A-2 synthesized in Example 1. [Diagram 5]1 is a result of 13C-NMR measurement of the methacrylate-modified phenolic resin A-2 synthesized in Example 1. [Figure 6] 1 shows the results of FD-MS measurement of the methacrylate-modified phenolic resin A-2 synthesized in Example 1. [Figure 7] 1 shows the results of GPC measurement of phenol resin B-1 synthesized in Example 2. [Figure 8] 1 shows the results of 13C-NMR measurement of the phenol resin B-1 synthesized in Example 2. [Figure 9] 1 shows the results of FD-MS measurement of phenol resin B-1 synthesized in Example 2. [Figure 10] 1 shows the results of GPC measurement of the methacrylate-modified phenolic resin B-2 synthesized in Example 2. [Figure 11] 1 is a result of 13C-NMR measurement of the methacrylate-modified phenolic resin B-2 synthesized in Example 2. [Figure 12] 1 shows the results of FD-MS measurement of the methacrylate-modified phenolic resin B-2 synthesized in Example 2. [Figure 13] 1 shows the results of GPC measurement of phenol resin C-1 synthesized in Example 3. [Figure 14] 1 shows the results of 13C-NMR measurement of phenol resin C-1 synthesized in Example 3. [Figure 15] 1 shows the results of FD-MS measurement of phenol resin C-1 synthesized in Example 3. [Figure 16] 1 shows the results of GPC measurement of the methacrylate-modified phenolic resin C-2 synthesized in Example 3. [Figure 17] 1 shows the results of 13C-NMR measurement of the methacrylate-modified phenolic resin C-2 synthesized in Example 3. [Figure 18] 1 shows the results of FD-MS measurement of the methacrylate-modified phenolic resin C-2 synthesized in Example 3. [Figure 19] 1 shows the results of GPC measurement of phenol resin D-1 synthesized in Example 4. [Figure 20] 1 shows the results of 13C-NMR measurement of the phenolic resin D-1 synthesized in Example 4. [Figure 21] 1 shows the results of FD-MS measurement of the phenolic resin D-1 synthesized in Example 4. [Figure 22] 1 shows the results of GPC measurement of the methacrylate-modified phenolic resin D-2 synthesized in Example 4. [Figure 23] 1 shows the results of 13C-NMR measurement of the methacrylate-modified phenolic resin D-2 synthesized in Example 4. [Figure 24] 1 shows the results of FD-MS measurement of the methacrylate-modified phenolic resin D-2 synthesized in Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, the mode for carrying out the invention will be described in detail, however, the present invention is not limited to the following description and can be carried out in various modified forms within the scope of the gist thereof.

[0010] [term] In this specification, the term "reaction raw material" refers to a compound that is used to obtain a target compound through a chemical reaction such as synthesis or decomposition and that partially constitutes the chemical structure of the target compound, and excludes substances that play the role of chemical reaction assistants such as solvents and catalysts. In particular, in this specification, the term "reaction raw material" refers to a precursor for obtaining a phenolic resin, which is a reaction product, through a chemical reaction. The term "structural unit" as used herein refers to a (repeating) unit of a chemical structure formed during a reaction or polymerization, in other words, refers to a partial structure other than the structure of the chemical bonds involved in the reaction or polymerization in a product compound formed by a reaction or polymerization, i.e., a so-called residue.

[0011] The aliphatic hydrocarbon group in this specification may be any of linear, branched and cyclic types, and may have an unsaturated bond in the structure. Examples of the aliphatic hydrocarbon group include those having 1 to 20 carbon atoms. In this specification, the monovalent aliphatic hydrocarbon group includes an alkyl group, an alkenyl group, an alkynyl group, a cycloalkyl group, a cycloalkenyl group, and a cycloalkynyl group. The alkyl group in this specification may be either a straight-chain or branched type and includes those having 1 to 20 carbon atoms, such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, a sec-pentyl group, a tert-pentyl group, a neopentyl group, an amyl group, a cyclopentyl group, a hexyl group, a heptyl group, an octyl group, a cumyl group, a nonyl group, a decyl group, an undecyl group, and a dodecyl group. The alkenyl group in this specification may be either a straight-chain or branched type and includes those having 2 to 20 carbon atoms, such as a vinyl group, an allyl group, a butenyl group, a butadienyl group, a pentenyl group, a hexenyl group, a heptenyl group, an octenyl group, a nonenyl group, a decenyl group, an undecenyl group, and a dodecenyl group. The alkynyl group in this specification may be either a straight-chain or branched type and includes those having 2 to 20 carbon atoms, such as an ethynyl group, a propargyl group, a butynyl group, a pentynyl group, a hexynyl group, a heptynyl group, an octynyl group, a nonynyl group, a decynyl group, an undecynyl group, and a dodecynyl group. The cycloalkyl group in this specification may be a monocyclic group or a polycyclic group and includes those having 3 to 30 carbon atoms, such as a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, an adamantyl group, a methylcyclohexyl group, and an ethylcyclohexyl group. The cycloalkenyl group in this specification may be a monocyclic group or a polycyclic group, and examples of the cycloalkenyl group include those having 3 to 30 carbon atoms, such as a cyclohexenyl group, a methylcyclohexenyl group, and an ethylcyclohexenyl group. The cycloalkynyl group in this specification may be a monocyclic group or a polycyclic group, and examples of the cycloalkynyl group include those having 4 to 30 carbon atoms, such as a cyclohexynyl group, a methylcyclohexynyl group, and an ethylcyclohexynyl group. In this specification, the divalent aliphatic hydrocarbon group includes an alkylene group, an alkenylene group, an alkynylene group, a cycloalkylene group, a cycloalkenylene group, and a cycloalkynylene group. The alkylene group in this specification may be either a straight-chain or branched type and includes those having 1 to 20 carbon atoms, such as a methylene group, ethylene group, propylene group, butylene group, pentylene group, hexylene group, heptylene group, octylene group, nonylene group, decylene group, undecylene group, and dodecylene group. The alkenylene group in this specification may be either a straight-chain or branched type and includes those having 2 to 20 carbon atoms, such as a vinylene group, a propenylene group, a butenylene group, a butadienylene group, an octenylene group, a decenylene group, and a dodecenylene group. The alkynylene group in this specification may be either a straight-chain or branched type and includes those having 2 to 20 carbon atoms, such as an ethynylene group, a propynylene group, a butynylene group, a butazinylene group, a pentynylene group, a hexynylene group, a heptynylene group, an octynylene group, a nonynylene group, a decynylene group, an undecynylene group, or a dodecynylene group. In the present specification, an alkoxy group has an alkyl-O- structure, and the above description of the alkyl group is applied to the alkyl portion in the structure, such as a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, an n-butoxy group, a sec-butoxy group, a tert-butoxy group, an allyloxy group, etc. The cycloalkylene group in this specification may be a monocyclic group or a polycyclic group, and can be one having 3 to 30 carbon atoms, such as a divalent group corresponding to the groups exemplified as the cycloalkyl group. The cycloalkenylene group in this specification may be a monocyclic group or a polycyclic group, and can be one having 3 to 30 carbon atoms, such as a divalent group corresponding to the groups exemplified as cycloalkenyl groups. The cycloalkynylene group in this specification may be a monocyclic group or a polycyclic group, and can be one having 4 to 30 carbon atoms, such as a divalent group corresponding to the groups exemplified as cycloalkynyl groups. The aromatic ring in this specification is a hydrocarbon ring consisting of a single ring or condensed rings having aromaticity, and includes those having 6 to 20 carbon atoms, such as a benzene ring, a naphthalene ring, an indene ring, an anthracene ring, an adamantane ring, etc. The aromatic ring group is a residue of an aromatic ring. The aryl group in this specification is a monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms, such as a phenyl group, a naphthyl group, a biphenyl group, or a phenanthryl group. In the present specification, the arylalkyl group is an alkyl group substituted with one or more, preferably one or two, particularly one, aryl group, and the above description of the aryl group and alkyl group applies to the aryl group and alkyl group, such as a benzyl group or a phenethyl group. Halogen atoms in this specification are fluorine, chlorine, bromine and iodine.

[0012] In this specification, the (meth)acrylate-modified phenolic resin is a resin in which at least a part of the phenolic hydroxyl groups of the phenolic resin is modified to a (meth)acrylate group ((meth)acryloyl group). (Meth)acrylic is a general term including acrylic and methacrylic, and similar expressions are the same. The number average molecular weight (Mn) and weight average molecular weight (Mw) in this specification are values ​​measured using gel permeation chromatography (hereinafter abbreviated as "GPC") under the measurement conditions described in the examples described later. The vinyl equivalent in this specification is a value calculated from the hydroxyl equivalent. Here, the hydroxyl equivalent is a value measured by titration. Here, the titration refers to the neutralization titration method in accordance with JIS K 0070.

[0013] The (meth)acrylate-modified phenolic resin of the present invention is a (meth)acrylic acid ester of a reaction product of a fluorene compound (provided that it does not have a substituent at the 9-position), a phenolic hydroxyl group-containing compound, and a compound represented by general formula (1). The reaction product of a fluorene compound (provided that it does not have a substituent at the 9-position), a phenolic hydroxyl group-containing compound, and a compound represented by general formula (1) is a phenolic resin, and can be said to be an intermediate of the (meth)acrylate-modified phenolic resin of the present invention.

[0014] [Reactive raw material for phenolic resin] The intermediate phenolic resin is a fluorene compound (not having a substituent at the 9-position) (hereinafter, also referred to simply as a "fluorene compound"), a phenolic hydroxyl group-containing compound, and a compound represented by the general formula (1) (wherein Ar is Ar 1 -Y-Ar 1 The reaction raw material is a compound represented by the general formula (1)

[0015] <Fluorene compounds> The fluorene compound is not particularly limited as long as it does not have a substituent at the 9-position of the fluorene, and may be unsubstituted or substituted at a position other than the 9-position.

[0016] The fluorene compound may be a compound represented by the following general formula (2). [ka] (where: m is independently an integer of 0 to 4, R 2 are each independently an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom.

[0017] The aliphatic hydrocarbon group is preferably an alkyl group having 1 to 4 carbon atoms, such as a methyl group, an ethyl group, a propyl group, or a butyl group. The aryl group is preferably a phenyl group, a tolyl group, a xylyl group, a naphthyl group, an indenyl group, or an indanyl group. The arylalkyl group is preferably a benzyl group, a phenethyl group, or a cumyl group. The alkoxy group is preferably a methoxy group, an ethoxy group, a propoxy group, or a butoxy group. The halogen atom is preferably fluorine, chlorine or bromine.

[0018] Each m is independently preferably an integer of 0 to 2, more preferably 0 or 1, and particularly preferably 0. The two m's may be the same or different, but are preferably the same. When both of the two m's are 1 or more, R substituted on the two benzene rings constituting the fluorene skeleton 2 may be the same or different. When either or both of m is 2 or more, two or more R 2 may be the same or different.

[0019] The compound of the general formula (2) is preferably fluorene. [ka]

[0020] The compound of formula (2) can be used alone or in combination of two or more kinds in any ratio.

[0021] <Phenol-containing hydroxyl group compounds> The phenolic hydroxyl group-containing compound is a compound having one phenolic hydroxyl group in the molecule.

[0022] An example of the phenolic hydroxyl group-containing compound is a compound represented by the following general formula (3). [ka] (where: n'' is an integer from 0 to 4, R 3’’ are each independently an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, or two R 3’’ may form a ring together with the carbon atom to which they are attached.

[0023] The aliphatic hydrocarbon group is preferably an alkyl group having 1 to 4 carbon atoms, such as a methyl group, an ethyl group, a propyl group, or a butyl group. The aryl group is preferably a phenyl group, a tolyl group, a xylyl group, or a naphthyl group. The arylalkyl group is preferably a benzyl group, a phenethyl group, or a cumyl group. The alkoxy group is preferably a methoxy group, an ethoxy group, a propoxy group, or a butoxy group. The halogen atom is preferably fluorine, chlorine or bromine. R 3’’ Among these, an alkyl group or an aryl group is preferable.

[0024] Or, two R's 3’’ may form a ring together with the carbon atom to which they are bonded. Examples of the ring include a hydrocarbon ring having 6 to 20 ring-constituting atoms, such as a benzene ring, a naphthalene ring, an anthracene ring, an adamantane ring, an indane ring, and an indene ring. These rings may have a substituent, and examples of the substituent include an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom.

[0025] n'' is preferably 0, 1 or 2. If n'' is 2, then two R 3’’ preferably form a benzene or naphthalene ring together with the carbon atom to which they are attached.

[0026] Preferred examples of the compound of formula (3) include the following compounds: [ka]

[0027] The compound of formula (3) can be used alone or in combination of two or more kinds in any ratio.

[0028] <Compound represented by general formula (1)> The compound represented by general formula (1) is a compound that can modify the hydrogen atom at the 9-position of the fluorene structural unit to an aralkyl, and can also react with a compound containing a phenolic hydroxyl group, and thus functions as a binder. [ka] (where: Ar is Ar 1 -Y-Ar 1 Or Ar 1 and Ar 1 each independently represents an aromatic ring group which may have a substituent, Y is a single bond, an aliphatic hydrocarbon group having 1 to 6 carbon atoms, -P(=O)R a - group, oxygen atom, sulfur atom or sulfonyl group, R a is an aromatic ring group, R 1 each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 4 carbon atoms, X is a leaving group.

[0029] Ar 1 is an aromatic ring group which may have a substituent. The aromatic ring group is not particularly limited, and is preferably a phenylene group, a naphthylene group, or an anthracenylene group. In the case of a phenylene group, it is preferable that the bonds are located at the 1- and 4-positions, in the case of a naphthylene group, it is preferable that the bonds are located at the 2- and 6-positions, and in the case of an anthracenylene group, it is preferable that the bonds are located at the 9- and 10-positions. Ar 1 -Y-Ar 1 Two Ar in 1may be the same or different, but is preferably the same.

[0030] Examples of the substituent include an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, and a halogen atom. The aliphatic hydrocarbon group is preferably an alkyl group having 1 to 4 carbon atoms, such as a methyl group, an ethyl group, a propylene group, or a butylene group. The aryl group is preferably a phenyl group, a tolyl group, a xylyl group, or a naphthyl group. The arylalkyl group is preferably a benzyl group, a phenethyl group, or a cumyl group. The alkoxy group is preferably a methoxy group, an ethoxy group, a propoxy group, or a butoxy group. The halogen atom is preferably fluorine, chlorine or bromine. Among them, the substituent is preferably an alkyl group, an aryl group, or the like.

[0031] Y is a single bond, an aliphatic hydrocarbon group having 1 to 6 carbon atoms, -P(=O)R a - group, an oxygen atom, a sulfur atom or a sulfonyl group (-S(=O)2- group). The aliphatic hydrocarbon group having 1 to 6 carbon atoms is not particularly limited, and is preferably a methylene group, an ethylene group, a propylene group, an isopropylidene group, or a butylidene group. -P(=O)R a -R in the group a is an aromatic ring group, preferably a phenyl group. Among these, Y is preferably a single bond, an ethylene group, or a propylene group.

[0032] Ar 1 -Y-Ar 1 As the alkyl group, a biphenylene group and a binaphthylene group are preferable.

[0033] X is a leaving group, and examples thereof include a hydroxyl group, a halogen atom, and an alkoxy group. The halogen atom is preferably chlorine, bromine or iodine. The alkoxy group is preferably an alkoxy group having 1 to 4 carbon atoms, such as a methoxy group, an ethoxy group, a propyloxy group, or a butoxy group. Among these, X is preferably a chlorine atom, a bromine atom, an iodine atom, a hydroxyl group, or a methoxy group. The two X's may be the same or different.

[0034] R 1 is a hydrogen atom or an aliphatic hydrocarbon group having 1 to 4 carbon atoms. The aliphatic hydrocarbon group having 1 to 4 carbon atoms is not particularly limited, and a methyl group, an ethyl group, a propyl group, a butyl group, and the like are preferred. R 1 Among them, hydrogen atom and methyl are preferable. 1 may be the same or different, but is preferably the same.

[0035] The compound of general formula (1) is a compound represented by the following general formula (1-1) (wherein Ar is Ar 1 -Y-Ar 1 and a compound of general formula (1-2) (Ar is Ar 1 ) is included. [ka] (where R 1 , Ar 1 The definitions and preferred examples of Y and X are as described above.

[0036] The compound of general formula (1) may be used alone or in combination of two or more kinds. That is, the compound of general formula (1) is a compound of general formula (1-1), a compound of general formula (1-2), or a combination of the compound of general formula (1-1) and the compound of general formula (1-2). The compound of general formula (1-1) and the compound of general formula (1-2) may be used alone or in combination of two kinds. When the compounds of general formula (1-1) and general formula (1-2) are used alone or in combination, the (meth)acrylate-modified phenolic resin is highly expressed in low dielectric tangent and low thermal expansion coefficient in a high temperature range. When the compound of general formula (1-1) and the compound of general formula (1-2) are used in combination, although there is no particular limitation, their molar ratio (molar number of the compound of general formula (1-1):molar number of the compound of general formula (1-2)) can be 10:90 to 90:10, preferably 20:80 to 80:20.

[0037] Preferred examples of the compound of formula (1-1) include the following. [ka]

[0038] Preferred examples of the compound of formula (1-2) include the following: [ka]

[0039] [Method of manufacturing phenolic resin] The intermediate phenol resin is obtained by reacting reactant materials, and specific production methods include the following.

[0040] The amounts of the reaction raw materials, fluorene compound, phenolic hydroxyl group-containing compound and compound of general formula (1), used are as follows: From the viewpoint of introducing a phenolic hydroxyl group-containing compound, the amount of the compound of general formula (1) may be more than 1 mole relative to 1 mole of the fluorene compound, and is not particularly limited as long as it is more than 1 mole. For example, the amount of the fluorene compound used may be 0.01 moles or more, preferably 0.1 moles or more, more preferably 0.3 moles or more, relative to 1 mole of the compound of general formula (1), and may be 0.99 moles or less, preferably 0.95 moles or less. During the reaction, substantially the entire amount of the fluorene compound and the compound of general formula (1) react, and therefore the molar ratio of the fluorene compound and the compound of general formula (1) used in the reaction is substantially the same as the molar ratio of the structural units derived from the fluorene compound and the structural units derived from the compound of general formula (1) in the obtained phenolic resin.

[0041] The amount of the phenolic hydroxyl group-containing compound used is not particularly limited, but may be an amount such that the amount of hydroxyl groups in the phenolic hydroxyl group-containing compound is 0.1 moles or more, preferably 0.2 moles or more, relative to the compound of general formula (1), and may be an amount such that the amount of hydroxyl groups in the phenolic hydroxyl group-containing compound is 10 moles or less, preferably 9.5 moles or less. Regarding the phenolic hydroxyl group-containing compound, some unreacted phenolic hydroxyl group-containing compound remains, but the amount of the reacted phenolic hydroxyl group-containing compound can be calculated from the hydroxyl group equivalent of the phenol resin.

[0042] A phenol resin, which is an intermediate, can be produced by the following steps 1 and 2.

[0043] <Process 1> It is preferable to react the entire amount of the fluorene compound and the entire amount of the compound of general formula (1) in an organic solvent using an alkali catalyst at 10 to 100°C without adding a phenolic hydroxyl group-containing compound, or to react the entire amount of the fluorene compound and the entire amount of the compound of general formula (1) with a part or the entire amount of the phenolic hydroxyl group-containing compound in an organic solvent using an alkali catalyst at 10 to 100°C.

[0044] The amount of the phenolic hydroxyl group-containing compound used is not particularly limited, but it can be an amount in which the hydroxyl group of the phenolic hydroxyl group-containing compound is 0.1 mol or more, preferably 0.2 mol or more, and can be an amount in which the hydroxyl group of the phenolic hydroxyl group-containing compound is 10 mol or less, preferably 9.5 mol or less, relative to the general formula (1). By using such an amount, the generation of by-products can be suppressed.

[0045] Examples of organic solvents include ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; aromatic hydrocarbon solvents such as toluene, xylene, mesitylene, and Solvesso; alcoholic solvents such as methanol, ethanol, 1-propyl alcohol, isopropyl alcohol, 1-butanol, sec-butanol, and tert-butanol; cellosolve solvents such as methyl cellosolve and ethyl cellosolve; ether solvents such as tetrahydrofuran, 1,4-dioxane, 1,3-dioxane, and diethoxyethane; and aprotic polar solvents such as acetonitrile, dimethyl sulfoxide, sulfolane, dimethylformamide, and dimethylacetamide. From the viewpoint of solubility, toluene, xylene, mesitylene, Solvesso, isopropyl alcohol, dimethyl sulfoxide, dimethylformamide, and dimethylacetamide are preferred. These organic solvents can be used alone or in combination of two or more at any ratio. The amount of the organic solvent used is not particularly limited, but is preferably 50 to 500% by mass based on the total amount of the compound of general formula (1) and the fluorene compound charged.

[0046] Examples of the alkali catalyst include lithium hydroxide, sodium hydroxide, potassium hydroxide, sodium methoxy, sodium ethoxy, sodium tert-butoxy, potassium methoxy, potassium ethoxy, potassium tert-butoxy, triethylamine, pyridine, and dimethylaminopyridine. From the viewpoint of reactivity, sodium hydroxide or potassium hydroxide is preferred. The amount of the alkali catalyst used can be 10 to 1000 mol% based on the amount of the general formula (1) charged. These catalysts can be used as an aqueous solution of 1 to 50 mass%.

[0047] A phase transfer catalyst may be used in the reaction. Examples of the phase transfer catalyst include ammonium-based catalysts such as tetrabutylammonium chloride, tetrabutylammonium bromide, tetrabutylammonium, tetrabutylammonium iodide, tetrabutylammonium hydroxide, benzyltriethylammonium chloride, benzyltriethylammonium bromide, benzyltriethylammonium iodide, and benzyltriethylammonium hydroxide; phosphonium-based catalysts such as tetrabutylphosphonium chloride, tetrabutylphosphonium bromide, tetrabutylphosphonium iodide, and tetrabutylphosphonium hydroxide; and crown ether-based catalysts such as 12-crown-4-ether, 15-crown-5-ether, 18-crown-6-ether, and tribenzo-18-crown-6-ether. In terms of reactivity, tetrabutylammonium bromide, tetrabutylammonium iodide, benzyltriethylammonium chloride, and benzyltriethylammonium iodide are preferred. The phase transfer catalyst may be used alone or in combination of two or more.

[0048] Additives may be used to promote the reaction. Examples of additives include halides such as lithium bromide, sodium bromide, potassium bromide, cesium bromide, lithium iodide, sodium iodide, potassium iodide, and cesium iodide. Among these, sodium iodide and potassium iodide are preferred. The additives may be used alone or in combination of two or more.

[0049] The reaction temperature can be from 10 to 100° C., and from the viewpoint of reactivity, is preferably from 20 to 80° C. The reaction time can be from 1 to 72 hours, and is preferably from 2 to 70 hours.

[0050] After the reaction is completed, the reaction mixture is separated into upper and lower layers as appropriate, and the lower layer, which is the aqueous layer, is removed to obtain the reaction product. At this time, water may be added as necessary to dissolve the insoluble salt and remove the lower layer. The aqueous layer may be basic, neutralized by neutralization, or acidic. Examples of neutralizing agents used for neutralization include inorganic acids such as hydrochloric acid, sulfuric acid, phosphoric acid, sodium monophosphate, and ammonium chloride, and organic acids such as methanesulfonic acid, paratoluenesulfonic acid, and oxalic acid. These acid catalysts may be used alone or in combination of two or more.

[0051] <Process 2> In the case where no phenolic hydroxyl group compound is added or a portion of the compound is added in step 1, the entire amount or the remainder of the phenolic hydroxyl group-containing compound is added to the reaction product obtained in step 1, and the reaction is carried out in the presence of an acid catalyst at 60 to 250° C. In the case where the entire amount of the phenolic hydroxyl group compound is added in step 1, the reaction product obtained in step 1 is reacted in the presence of an acid catalyst at 60 to 250° C.

[0052] The phenolic hydroxyl group-containing compound used in step 2 may be the same as or different from the phenolic hydroxyl group-containing compound used in step 1.

[0053] Examples of the acid catalyst include inorganic acids such as hydrochloric acid, sulfuric acid, and phosphoric acid, organic acids such as methanesulfonic acid, paratoluenesulfonic acid, and oxalic acid, and Lewis acids such as boron trifluoride, aluminum chloride, and zinc chloride. From the viewpoint of solubility, paratoluenesulfonic acid and methanesulfonic acid are preferred. These acid catalysts may be used alone or in combination of two or more. The amount of the acid catalyst is not particularly limited, but is preferably 0.001 to 10% by mass based on the total amount of the reaction raw materials charged.

[0054] The reaction temperature is 60 to 250° C., and from the viewpoint of reactivity, is preferably 80 to 240° C. The reaction time can be 1 to 72 hours, and is preferably 2 to 70 hours.

[0055] After the reaction is completed, neutralization and washing with water are carried out as necessary, and unreacted reactants, organic solvents, etc. are distilled off under reduced pressure and heating conditions to obtain a phenolic resin as an intermediate.

[0056] The method for producing the intermediate phenolic resin is not limited to the above. For example, instead of step 1, a fluorene compound and a compound of general formula (1) may be reacted in an organic solvent in the presence of a catalyst at 10 to 100°C, and then a part of a phenolic hydroxyl group-containing compound may be added and reacted at 10 to 100°C, after which the water layer is removed, a water washing treatment is performed, and the resulting reaction product may be subjected to step 2. In this case, the reaction product of step 1 may have a reactive group at the end, and the reactive group may be an ether reacted with a phenol, a halide, a hydroxyl group, or an ether reacted with an alcohol-based solvent, depending on the type of compound used.

[0057] [Phenol resin] The intermediate phenolic resin is a reaction product of a fluorene compound, a phenolic hydroxyl group-containing compound, and a compound of general formula (1).

[0058] The fluorene compound represented by general formula (2), the phenolic hydroxyl group-containing compound represented by general formula (3), and the compound of general formula (1) can respectively produce a structural unit represented by general formula (2A) or general formula (2A'), a structural unit represented by general formula (3A) or general formula (3A'), and a structural unit represented by general formula (1A). [ka] (wherein the definition, examples and preferred examples of m and m' are the same as those of m in general formula (2), R 2 and R 2’ The definition, examples and preferred examples of R in the general formula (2) are as follows:2 is the same as * represents a bond.) [ka] (where: n is an integer from 0 to 3, preferably 0, 1 or 2. n' is an integer of 0 to 4, preferably 0, 1 or 2; R 3 and R 3’ The definition, examples and preferred examples of are the same as those of R″ in general formula (3). * represents a bond.) [ka] (where: Ar and R 1 The definition, examples and preferred examples are the same as those of general formula (1), * represents a bond.)

[0059] The intermediate phenol resin contains a structure in which the structural unit of general formula (1A) is bonded to the structural unit of general formula (2A) and / or general formula (2A'). At least one molecular chain terminal of the intermediate phenolic resin is preferably a structural unit of general formula (3A'), and both molecular chain terminals are preferably structural units of general formula (3A').

[0060] The intermediate phenolic resin is composed of structural units of general formula (2A) and / or general formula (2A'), structural units of general formula (3A) and / or (3A'), and structural units of general formula (1A), with the proviso that the bonds of the structural units of general formula (2A) and / or general formula (2A') may be bonded to bonds of the structural units of general formula (1A). When general formula (2A') is present, the structural units of the structural units constitute the molecular chain terminals. At least one of the molecular chain terminals is preferably a structural unit of general formula (3A'), and more preferably both of the molecular chain terminals are structural units of general formula (3A').

[0061] In the structural unit of the general formula (1A) in the intermediate phenolic resin, Ar is Ar1 or Ar 1 -Y-Ar 1 In other words, all of the Ar contained in the intermediate phenolic resin is Ar 1 or Ar 1 -Y-Ar 1 or Ar 1 -Y-Ar 1 and Ar 1 The intermediate phenolic resin can be made up of Ar 1 and Ar 1 -Y-Ar 1 Among them, the incorporation of at least one of them is preferred because it leads to the high expression of a low dielectric tangent and a low thermal expansion coefficient in a high temperature range in the methacrylate modified phenolic resin. 1 -Y-Ar 1 and Ar 1 When the compound is composed of the above, the molar ratio of the above (Ar 1 -Y-Ar 1 Number of moles of Ar 1 The molar ratio of the two components (molar ratio) can be 10:90 to 90:10, and is preferably 20:80 to 80:20.

[0062] The structural unit of the general formula (1A) is 1 -Y-Ar 1 or Ar is a structural unit represented by the following general formula (1-1A): 1 or the structural unit of the following general formula (1-1A) and Ar are Ar 1 It is preferable that Ar is composed of the structural unit of the following general formula (1-1A) and the structural unit of the following general formula (1-2A), because this leads to a high degree of expression of a low dielectric tangent and a low thermal expansion coefficient in a high temperature region in the methacrylate-modified phenolic resin.

[0063] [ka] (where R 1 , Ar 1 The definitions and preferred examples of Y and X are the same as those of general formula (1), * represents a bond.)

[0064] When the structural unit of general formula (1A) is composed of a structural unit of general formula (1-1A) and a structural unit of general formula (1-2A), the molar ratio therebetween (the number of moles of the structural unit of general formula (1-1A):the number of moles of the structural unit of general formula (1-2)) is not particularly limited, but may be 10:90 to 90:10, and preferably 20:80 to 80:20.

[0065] Preferred examples of the structural unit of general formula (1-1A) are as follows: [ka]

[0066] Preferred examples of the compound of formula (1-2) include the following: [ka]

[0067] An example of the intermediate phenol resin is a phenol resin represented by the following general formula (5). [ka] (where: Z is independently a group represented by the general formula (2A): [ka] or a structural unit represented by general formula (3A): [ka] It is a structural unit represented by Z' is independently a group represented by the general formula (2A'): [ka] or a structural unit represented by general formula (3A'): [ka] It is a structural unit represented by Ar is independently Ar 1 Or Ar 1 -Y-Ar 1 and Ar 1 each independently represents an aromatic ring group which may have a substituent, Y is a single bond, an aliphatic hydrocarbon group having 1 to 6 carbon atoms, -P(=O)R a - group, oxygen atom, sulfur atom or sulfonyl group, R a is an aromatic ring group, R 1 each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 4 carbon atoms, R 2 each independently represents an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, m is independently an integer of 0 to 4, R 3 are each independently an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, or two R 3 may form a ring together with the carbon atom to which they are attached, n is independently an integer of 0 to 3, R 2’ each independently represents an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, m' is independently an integer of 0 to 4, R 3’ are each independently an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, or two R 3’ may form a ring together with the carbon atom to which they are attached, Each n' is independently an integer of 0 to 4, p is an average value greater than 0; however, The resin contains a structural unit represented by general formula (2A) and / or general formula (2A') and a structural unit represented by general formula (3A) and / or general formula (3A').

[0068] In the above, Ar, Ar 1 , Y, R 1 、 R 2 , R 3 , m, n, R 2’ , R 3’ , m', n' and p are the same as those described above. 1 and Ar 1 -Y-Ar 1 The examples and preferred examples are the same as those mentioned above.

[0069] The phenolic resin of general formula (5) is a mixture of compounds in which p in the above general formula (5) is an integer of 0 or more (provided that not all of the compounds are compounds of general formula (5) in which p is 0), and preferably includes a compound containing both structural units represented by general formula (2A) and / or general formula (2A') and structural units represented by general formula (3A) and / or general formula (3A') in the molecule. In the resin, the total amount of the structural units of general formulae (2A) and (2A') is preferably 0.1 to 10 mol, more preferably 0.5 to 9.5 mol, per 1 mol of the structural units of general formulae (3A) and (3A').

[0070] A preferred example is a phenol resin represented by the following general formula (5-0). [ka] (Wherein, Ar, Y, R 1 , R 3’ , n' and p are the same as in general formula (5).

[0071] Where Ar, Y, R 1 , R 3 , n' and p are the same as those described above. 1 and Ar 1 -Y-Ar 1 The examples and preferred examples of are the same as those described above. R in Z 2 , m, R 3 Examples and preferred examples of n are the same as those mentioned above.

[0072] A more preferred example of the phenol resin of the present invention is a phenol resin represented by the following general formula (5-0'). [ka] (where R 2 , m, R 3 , n, R 3’ and n' is as defined above; Ar' is [ka] and s is the average value, a number greater than 0; t is the average value, and is a number equal to or greater than 0; The order of the structural units bracketed by s and the structural units bracketed by t is not limited.

[0073] The phenolic resin of general formula (5) and the phenolic resin of general formula (5-0) may be a mixture of compounds each having a structural unit bounded by p with an integer of 0 or more, but not all of the compounds are compounds of general formula (5) in which p is 0. The phenolic resin of general formula (5) preferably contains at least one of the compounds represented by general formula (5-1) and general formula (5-2). [ka] (where: Ar, Z, R 1 , R 3‘ and n' are as defined above; Z in general formula (5-1) and at least one Z in general formula (5-2) are structural units represented by general formula (2A).

[0074] The intermediate phenol resin may contain a compound of general formula (6) as a part thereof. The compound of general formula (6) corresponds to the compound of general formula (5) in which p is 0. [ka] (where: Ar, R 1 , R 3’ and n' are as defined above.

[0075] The number average molecular weight (Mn) of the phenolic resin, which is an intermediate, can be in the range of 100 to 10,000, and preferably in the range of 200 to 8,000. The weight average molecular weight (Mw) of the phenolic resin can be in the range of 100 to 50,000, and preferably in the range of 300 to 40,000. The molecular weight distribution (weight average molecular weight (Mw) / number average molecular weight (Mn)) of the phenol resin intermediate can be in the range of 1-5, and is preferably 1-4.

[0076] The hydroxyl equivalent of the phenolic resin intermediate is preferably in the range of 100-2,000, and more preferably 200-1,800.

[0077] [Method for producing (meth)acrylate modified phenolic resin] The (meth)acrylate-modified phenolic resin of the present invention is a (meth)acrylic acid ester of an intermediate phenolic resin, and can be obtained, for example, by reacting an intermediate phenolic resin with a (meth)acrylation agent in the presence of a basic or acidic catalyst.

[0078] The (meth)acrylation agent is not particularly limited as long as it is a compound capable of reacting with the hydroxyl group of the phenolic resin to introduce a (meth)acryloyl group. Examples of the (meth)acrylation agent include (meth)acrylic anhydride, (meth)acrylic acid chloride, (meth)acrylic acid, and (meth)acrylic acid esters. Examples of the (meth)acrylic acid esters include alkyl esters of (meth)acrylic acid (e.g., alkyl esters having 1 to 4 carbon atoms). (Meth)acrylic anhydride includes methacrylic anhydride and acrylic anhydride, (meth)acrylic chloride includes methacrylic chloride and acrylic chloride. (Meth)acrylic acid includes methacrylic acid and acrylic acid, and (meth)acrylic acid esters include methacrylic acid esters and acrylic acid esters. When the (meth)acrylation agent is methacrylic anhydride, methacrylic acid chloride, methacrylic acid, methacrylic acid esters, etc., a methacryloyl group is introduced, and when the (meth)acrylation agent is acrylic anhydride, acrylic acid chloride, acrylic acid, acrylic acid esters, etc., an acryloyl group is introduced.

[0079] The reaction between the intermediate phenol resin and the (meth)acrylation agent is preferably carried out using 0.3 to 10 moles of the (meth)acrylation agent per mole of hydroxyl groups contained in the intermediate phenol resin.

[0080] Examples of basic catalysts include amine-containing catalysts such as trimethylamine, triethylamine, N,N-diisopropylmethylamine, 1,8-diazabicyclo[5,4,0]-7-undecene, 1,5-diazabicyclo[4,3,0]-5-nonene, pyridine, and dimethylaminopyridine, alkaline earth metal hydroxides such as calcium hydroxide and barium hydroxide, alkali metal carbonates such as sodium carbonate and potassium carbonate, and alkali metal hydroxides such as sodium hydroxide and potassium hydroxide. Examples of acidic catalysts include sulfuric acid, methanesulfonic acid, and p-toluenesulfonic acid. Among them, triethylamine, N,N-diisopropylmethylamine, dimethylaminopyridine, and pyridine are preferred from the viewpoint of catalytic activity. The above catalysts may be used alone or in combination of two or more.

[0081] In the reaction, it is preferable to use 0.3 to 10 moles of a basic or acidic catalyst per mole of hydroxyl groups contained in the intermediate phenolic resin. These catalysts may be added all at once or in portions.

[0082] The reaction temperature can be from 20 to 150° C. The reaction time can be from 1 to 72 hours.

[0083] The reaction is preferably carried out in an organic solvent. Examples of the organic solvent include ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; aromatic hydrocarbon solvents such as toluene, xylene, mesitylene, and Solvesso; alcoholic solvents such as methanol, ethanol, 1-propyl alcohol, isopropyl alcohol, 1-butanol, sec-butanol, and tert-butanol; cellosolve solvents such as methyl cellosolve and ethyl cellosolve; ether solvents such as tetrahydrofuran, 1,4-dioxane, 1,3-dioxane, and diethoxyethane; and aprotic polar solvents such as acetonitrile, dimethyl sulfoxide, sulfolane, dimethylformamide, and dimethylacetamide. From the viewpoint of solubility, toluene, xylene, mesitylene, Solvesso, isopropyl alcohol, dimethyl sulfoxide, dimethylformamide, and dimethylacetamide are preferred. These organic solvents can be used alone or in combination of two or more at any ratio. The amount of the organic solvent used is not particularly limited, but is preferably 50 to 700% by mass based on the total amount of the charged intermediate phenol resin and (meth)acrylation agent.

[0084] After the reaction is completed, the (meth)acrylate-modified phenolic resin of the present invention can be obtained by carrying out reprecipitation, recrystallization, washing with water, distillation, etc.

[0085] [(Meth)acrylate modified phenolic resin] The (meth)acrylate-modified phenolic resin of the present invention is a (meth)acrylic acid ester of an intermediate phenolic resin, and is a (meth)acrylic acid-modified phenolic resin in which a (meth)acryloyl group is introduced into the phenolic hydroxyl group.

[0086] The (meth)acrylate-modified phenolic resin can be, for example, one represented by general formula (15). [ka] (where: Z is independently a group represented by the general formula (12A): [ka] or a structural unit represented by general formula (13A): [ka] It is a structural unit represented by Z' is independently a group represented by the general formula (12A'): [ka] or a structural unit represented by general formula (13A'): [ka] It is a structural unit represented by Ar is independently Ar 1 Or Ar 1 -Y-Ar 1 and Ar 1 each independently represents an aromatic ring group which may have a substituent, Y is a single bond, an aliphatic hydrocarbon group having 1 to 6 carbon atoms, -P(=O)R a - group, oxygen atom, sulfur atom or sulfonyl group, R a is an aromatic ring group, R 1 each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 4 carbon atoms, R 2 each independently represents an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, m is independently an integer of 0 to 4, R b are each independently a hydrogen atom or a methyl group, R 3 are each independently an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, or two R 3may form a ring together with the carbon atom to which they are attached, n is independently an integer of 0 to 3, R 2’ each independently represents an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, m' is independently an integer of 0 to 4, R b’ are each independently a hydrogen atom or a methyl group, R 3’ are each independently an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, or two R 3’ may form a ring together with the carbon atom to which they are attached, Each n' is independently an integer of 0 to 4, p is the average value and is a number greater than 0; however, The resin contains a structural unit represented by general formula (12A) and / or general formula (12A') and a structural unit represented by general formula (13A) and / or general formula (13A').

[0087] In the above, Ar, Ar 1 , Y, R 1 、 R 2 , R 3 , m, n, R 2’ , R 3’ , m', n' and p are the same as those described above. 1 and Ar 1 -Y-Ar 1 The examples and preferred examples are the same as those mentioned above.

[0088] R b and R b’ are each independently a hydrogen atom or a methyl group. In the case of a hydrogen atom, an acryloyl group is introduced into the phenolic hydroxyl group, and in the case of a methyl group, a methacryloyl group is introduced into the phenolic hydroxyl group.

[0089] The (meth)acrylate-modified phenolic resin of general formula (15) may be a mixture of compounds in which p in the above general formula (15) is an integer of 0 or more, but not all of the compounds are compounds of general formula (15) in which p is 0. It is preferable to include a compound containing both a structural unit represented by general formula (12A) and / or general formula (12A') and a structural unit represented by general formula (13A) and / or general formula (13A') in the molecule. In the resin, the total amount of structural units of general formulae (12A) and (12A') is preferably 0.1 to 10 mol, more preferably 0.5 to 9.5 mol, per 1 mol of the total of structural units of general formulae (13A) and (13A').

[0090] A preferred example is a phenol resin represented by the following general formula (15-0). [ka] (Wherein, Ar, Y, R 1 , R 3’ , n', p and R b’ is the same as general formula (15).

[0091] Where Ar, Y, R 1 , R 3 , n' p and R b’ The examples and preferred examples of are the same as those described above. 1 and Ar 1 -Y-Ar 1 The examples and preferred examples of are the same as those described above. R in Z 2 , m, R 3 Examples and preferred examples of n are the same as those mentioned above.

[0092] A more preferred example of the phenol resin of the present invention is a phenol resin represented by the following general formula (15-0'). [ka] (where R 2 , m, R3 , n, R 3’ , n' and R b’ is as above, Ar' is [ka] and s is the average value, a number greater than 0; t is the average value, and is a number equal to or greater than 0; The order of the structural units bracketed by s and the structural units bracketed by t is not limited.

[0093] The (meth)acrylate-modified phenolic resin of general formula (15) and the (meth)acrylate-modified phenolic resin of general formula (15-0) may each be a mixture of compounds having a structural unit bounded by p with an integer of 0 or more (provided that not all of the compounds are compounds of general formula (15) in which p is 0). The phenolic resin of general formula (15) preferably contains at least one of the compounds represented by general formula (15-1) and general formula (15-2). [ka] (where: Ar, Z, R 1 , R 3’ , n' and R b’ is as above, Z in general formula (15-1) and at least one Z in general formula (15-2) are structural units represented by general formula (2A).

[0094] The (meth)acrylate-modified phenolic resin may contain a compound of general formula (16) as a part thereof. The compound of general formula (16) corresponds to the compound of general formula (15) above in which p is 0. [ka] (where: Ar, R 1 , R 3’ , n' and R b’is as above.)

[0095] The number average molecular weight (Mn) of the (meth)acrylate modified phenolic resin may be in the range of 100 to 10,000, and preferably in the range of 200 to 8,000. The weight average molecular weight (Mw) of the (meth)acrylate modified phenolic resin may be in the range of 100 to 50,000, and preferably in the range of 300 to 40,000. The molecular weight distribution (weight average molecular weight (Mw) / number average molecular weight (Mn)) of the (meth)acrylate-modified phenolic resin can be in the range of 1-5, and is preferably 1-4.

[0096] The vinyl equivalent of the (meth)acrylate modified phenolic resin is preferably in the range of 100 to 10,000, and more preferably 200 to 9,000.

[0097] [Curable composition] The curable composition of the present invention contains the (meth)acrylate-modified phenolic resin of the present invention. By using the (meth)acrylate-modified phenolic resin of the present invention, it is possible to achieve low dielectric tangent and high heat resistance in a cured product obtained from the curable composition.

[0098] The curable composition of the present invention may contain a polymerizable unsaturated group-containing compound other than the (meth)acrylate-modified phenolic resin. The other polymerizable unsaturated group-containing compound is not particularly limited, and a wide variety of compounds can be used.

[0099] Examples of other polymerizable unsaturated group-containing compounds include Monofunctional compounds such as styrene, alkoxy(poly)oxyalkylene(meth)acrylate, phenoxy(poly)oxyalkylene(meth)acrylate, and alkoxylated phenylphenol(meth)acrylate; Bifunctional compounds such as divinylbenzene, diallyl phthalate, diallyl isophthalate, diallyl terephthalate, aliphatic diol di(meth)acrylates having 2 to 12 carbon atoms, polyoxyalkylene di(meth)acrylates, tricyclodecane dimethanol di(meth)acrylate, and (poly)alkoxylated bisphenol di(meth)acrylates; Trifunctional or higher compounds such as trimethylolpropane tri(meth)acrylate, alkoxylated trimethylolpropane tri(meth)acrylate, glycerin (meth)acrylate, alkoxylated glycerin tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, alkoxylated pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, alkoxylated ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, alkoxylated dipentaerythritol hexa(meth)acrylate, triallyl isocyanurate, triallyl cyanurate, and tris-[2-(meth)acryloxyethyl]isocyanurate; Polymerizable unsaturated group-containing resins such as maleimide resins, unsaturated polyester resins, and polybutadiene resins; and the like. These may be used alone or in combination of two or more kinds.

[0100] The content of the (meth)acrylate-modified phenolic resin of the present invention relative to the total mass of the polymerizable unsaturated group-containing compound contained in the curable composition is preferably 30 mass% or more, more preferably 50 mass% or more, and even more preferably 60 mass% or more.

[0101] The curable composition of the present invention may contain other resins other than the other polymerizable unsaturated group-containing compounds. The other resins are not particularly limited, and a wide variety of resins having functional groups and specific structures can be used. For example, epoxy resins, phenolic resins, active ester resins, cyanate resins, etc. can be mentioned.

[0102] The curable composition may contain a curing catalyst. The curing catalyst is not particularly limited, and examples thereof include organic peroxides (e.g., benzoyl peroxide, cumene hydroperoxide, dicumyl peroxide, lauroyl peroxide, di-t-butyl peroxide, t-butyl hydroperoxide, methyl ethyl ketone peroxide, t-butyl perbenzoate, etc.), azo compounds (azobisisobutyronitrile, etc.), and free radicals (azobisisobutyronitrile, galvinoxyl, etc.).

[0103] The curable composition may contain various compounding agents such as a curing accelerator, a silane coupling agent, a release agent, a pigment, an emulsifier, a non-halogen-based flame retardant, an inorganic filler, a flame retardant (e.g., an inorganic phosphorus-based flame retardant, an organic phosphorus-based flame retardant, or a halogen-based flame retardant), and a solvent.

[0104] The curable composition can be obtained by uniformly mixing the (meth)acrylate-modified phenolic resin of the present invention and any optional components (for example, other polymerizable unsaturated group-containing compounds, other resins, curing catalysts, compounding agents, etc.).

[0105] [Cured product] The cured product of the present invention can be obtained by curing the curable composition of the present invention. The curing method is not particularly limited, and a known method can be adopted. The cured product can be in the form of a laminate, a cast product, an adhesive layer, a coating film, a film, etc.

[0106] [Semiconductor encapsulation materials] The semiconductor encapsulant of the present invention may contain the curable composition of the present invention. Since the curable composition of the present invention contains the (meth)acrylate-modified phenolic resin of the present invention, the semiconductor encapsulant containing the curable composition can exhibit a low dielectric tangent and a low thermal expansion coefficient.

[0107] The semiconductor encapsulant may be prepared by adding an inorganic filler to the curable composition of the present invention. The inorganic filler is not particularly limited, and examples thereof include barium sulfate, barium titanate, amorphous silica, crystalline silica, Neuburg silica, fused silica, spherical silica, talc, clay, magnesium carbonate, calcium carbonate, aluminum oxide, aluminum hydroxide, silicon nitride, and aluminum nitride. The amount of the inorganic filler may be 0.5 to 1200 parts by mass based on 100 parts by mass of the curable composition.

[0108] The semiconductor encapsulant may contain various compounding agents, including those described for the curable composition.

[0109] The semiconductor encapsulant can be obtained by mixing the curable composition of the present invention and, if necessary, compounding ingredients. For example, a method of thoroughly melt-mixing the composition using an extruder, kneader, roll, or the like until the composition becomes homogeneous can be mentioned.

[0110] [Semiconductor Devices] The semiconductor device of the present invention can include a cured product of the semiconductor encapsulant of the present invention. The semiconductor encapsulant used in the semiconductor device of the present invention contains a curable composition containing the (meth)acrylate-modified phenolic resin of the present invention. The semiconductor device of the present invention has a low dielectric tangent and a low thermal expansion coefficient because it includes a cured product of the semiconductor encapsulant.

[0111] A semiconductor device can be obtained by heating and curing the semiconductor encapsulant of the present invention, for example, by casting or molding using a transfer molding machine, injection molding machine, or the like, and then heating and curing in a temperature range of room temperature (20°C) to 250°C.

[0112] [Prepreg] The prepreg of the present invention may have a reinforcing substrate and a semi-cured product of the curable composition of the present invention impregnated into the reinforcing substrate. The method for obtaining a prepreg from the curable composition is not particularly limited, and examples thereof include a method in which the curable composition is made into a varnish by blending an organic solvent described later into the curable composition, which is then impregnated into a reinforcing base material (e.g., paper, glass cloth, glass nonwoven fabric, aramid paper, aramid cloth, glass mat, glass roving cloth, etc.), and then heated at a heating temperature (preferably 50 to 170°C) according to the type of solvent used to semi-cure (or uncure) the curable composition. The mass ratio between the curable composition and the reinforcing base material used is not particularly limited, but it is preferable to adjust the resin content in the prepreg to 20 to 60 mass %.

[0113] The semi-cured product of the curable composition can be obtained by adjusting the heating temperature and heating time to stop the curing reaction midway without completing it. The degree of curing of the semi-cured product can be, for example, 5% or more and 85% or less. Here, the cured product can have a higher degree of curing than the semi-cured product. The degree of curing of the semi-cured product can be calculated from the following formula by measuring the amount of heat generated during curing when the curable composition is heated and the amount of heat generated during curing of the semi-cured product by DSC. Degree of cure (%)=[1-(cure heat generation amount of semi-cured product / cure heat generation amount of curable composition)]×100

[0114] Examples of organic solvents used in the production of prepregs include methyl ethyl ketone, acetone, dimethylformamide, methyl isobutyl ketone, methoxypropanol, cyclohexanone, methyl cellosolve, ethyl diglycol acetate, propylene glycol monomethyl ether acetate, etc. The selection of the organic solvent and the amount used can be appropriately selected depending on the application, and for example, when producing a circuit board from a prepreg, polar solvents with a boiling point of 160° C. or less such as methyl ethyl ketone, acetone, dimethylformamide, etc. are preferred, and the amount used is preferably an amount such that the nonvolatile content is 40 to 80 mass%.

[0115] [Circuit board] The circuit board of the present invention is made of a laminate of the prepreg of the present invention and copper foil. The method for obtaining the circuit board is not particularly limited, and an example thereof is a method in which the prepreg of the present invention is laminated as necessary, copper foil is superimposed, and the laminate is heated and compressed at 170 to 300° C. under a pressure of 1 to 10 MPa for 10 minutes to 3 hours.

[0116] [Build-up film] The build-up film of the present invention may contain the curable composition of the present invention. The method for producing the build-up film is not particularly limited, and may be, for example, a method in which the curable composition of the present invention is applied onto a support film to form a curable composition layer to form an adhesive film for a multilayer printed wiring board.

[0117] The build-up film is required to soften under the temperature conditions for lamination in the vacuum lamination method (usually 70 to 140°C) and to exhibit fluidity (resin flow) that allows resin to fill via holes or through holes present in the circuit board at the same time as lamination of the circuit board. Therefore, it is preferable that the curable composition contains the above-mentioned components so as to exhibit such properties.

[0118] Here, the diameter of the through-holes in the multilayer printed wiring board is usually 0.1 to 0.5 mm, and the depth is usually 0.1 to 1.2 mm, and it is usually preferable to make it possible to fill the resin within this range. When both sides of the circuit board are laminated, it is preferable to fill about 1 / 2 of the through-holes.

[0119] Specifically, the adhesive film can be produced by preparing the curable composition in a varnish form, applying the varnish-like composition to the surface of the support film (Y), and then drying the organic solvent by heating or blowing hot air or the like to form a composition layer (X) made of the curable composition.

[0120] The thickness of the composition layer (X) formed is usually preferably equal to or greater than the thickness of the conductor layer. Since the thickness of the conductor layer of the circuit board is usually in the range of 5 to 70 μm, the thickness of the resin composition layer is preferably 10 to 100 μm.

[0121] The composition layer (X) may be protected with a protective film described below. By protecting the resin composition layer with a protective film, the surface of the resin composition layer can be prevented from being scratched or from being contaminated by dirt or the like.

[0122] Examples of the above-mentioned support film (Y) and protective film include polyolefins such as polyethylene, polypropylene, and polyvinyl chloride, polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate, polycarbonate, polyimide, and further release paper and metal foils such as copper foil and aluminum foil. The support film and protective film may be subjected to a release treatment in addition to a mud treatment and a corona treatment.

[0123] The thickness of the support film is not particularly limited, but is usually in the range of 10 to 150 μm, preferably 25 to 50 μm, and the thickness of the protective film is preferably 1 to 40 μm.

[0124] The above-mentioned support film (Y) is peeled off after laminating it onto the circuit board or after forming an insulating layer by heat curing. If the support film (Y) is peeled off after the adhesive film is heat cured, the adhesion of dust and the like during the curing process can be prevented. When peeling off after curing, the support film is usually subjected to a release treatment in advance.

[0125] [Application] The cured product obtained by the curable composition containing the (meth)acrylate-modified phenolic resin of the present invention has a low dielectric tangent and a low coefficient of thermal expansion, and therefore can be suitably used for heat-resistant members or electronic members. In particular, it can be suitably used for prepregs, circuit boards, semiconductor encapsulants, semiconductor devices, build-up films, build-up boards, adhesives using conductive pastes, resist materials, and the like. It can also be suitably used for the matrix resin of fiber-reinforced resins, and is particularly suitable as a highly heat-resistant prepreg. In addition, the (meth)acrylate-modified phenolic resin contained in the curable composition exhibits excellent solubility in various solvents, and can be made into a paint. The heat-resistant members and electronic members thus obtained can be suitably used for various applications, including, but not limited to, industrial machine parts, general machine parts, automobile, railway, and vehicle parts, space and aviation-related parts, electronic and electrical parts, building materials, containers and packaging materials, daily necessities, sports and leisure goods, and housing members for wind power generation. EXAMPLES

[0126] The present invention will be specifically described with reference to examples and comparative examples, but the present invention is not limited to the following description and can be practiced with various modifications within the scope of the gist. In the following, "parts" and "%" are based on mass unless otherwise specified.

[0127] The physical properties of the phenolic resin and the (meth)acrylate-modified phenolic resin were evaluated as follows.

[0128] (1) GPC measurement Using the following measuring equipment and conditions, the number average molecular weight (Mn), weight average molecular weight (Mw), and molecular weight distribution (Mw / Mn) of the phenolic resins and (meth)acrylate-modified phenolic resins obtained in the examples and comparative examples were calculated. "Measuring device" Tosoh Corporation "HLC-8320 GPC" "Measurement conditions" Column: Tosoh Corporation guard column "HXL-L" + Tosoh Corporation "TSK-GEL G2000HXL" + Tosoh Corporation "TSK-GEL G2000HXL" + Tosoh Corporation "TSK-GEL G3000HXL" + Tosoh Corporation "TSK-GEL G4000HXL" Detector: RI (differential refractometer) Data processing: Tosoh Corporation's "GPC Workstation EcoSEC-WorkStation" Measurement conditions: Column temperature 40℃ Developing solvent: Tetrahydrofuran Flow rate 1.0ml / min Standard: In accordance with the measurement manual for the "GPC Workstation EcoSEC-WorkStation," the following monodisperse polystyrene with known molecular weight was used. (Polystyrene used) "A-500" manufactured by Tosoh Corporation "A-1000" manufactured by Tosoh Corporation "A-2500" manufactured by Tosoh Corporation "A-5000" manufactured by Tosoh Corporation "F-1" manufactured by Tosoh Corporation "F-2" manufactured by Tosoh Corporation "F-4" manufactured by Tosoh Corporation "F-10" manufactured by Tosoh Corporation "F-20" manufactured by Tosoh Corporation "F-40" manufactured by Tosoh Corporation "F-80" manufactured by Tosoh Corporation "F-128" manufactured by Tosoh Corporation Sample: A tetrahydrofuran solution (1.0 mass % in terms of resin solid content) of the phenolic resin or (meth)acrylate-modified phenolic resin obtained in Synthesis Example was filtered through a microfilter (50 μl).

[0129] (2) FD-MS measurement The FD-MS spectra of the phenolic resins and (meth)acrylate-modified phenolic resins obtained in the examples were measured using the following measuring device and under the following measuring conditions. Measurement equipment: JMS-T100GC AccuTOF Measurement conditions Measurement range: m / z=4.00~2000.00 Rate of change: 51.2mA / min Final current value: 45mA Cathode voltage: -10kV Recording interval: 0.07 seconds

[0130] (3) 13 C-NMR measurement Phenolic resins and (meth)acrylate-modified phenolic resins obtained in the examples 13 C-NMR spectra were measured using the following measuring device and conditions. 13 C-NMR: “JNM-ECZ400S” manufactured by JEOL RESONANCE Resonance frequency: 100MHz Number of times: 4000 Solvent: Chloroform-d Sample concentration: 12% by mass Relaxation agent: Chromium(III) acetylacetonate

[0131] Example 1: Methacrylate-modified phenolic resin A-2 <Synthesis of phenolic resin A-1> A flask equipped with a thermometer, a dropping funnel, a condenser, a fractionating column, and a stirrer was charged with 100.0 parts by mass of fluorene, 226.6 parts by mass of 4,4'-bis(chloromethyl)biphenyl (BCMB), 14.6 parts by mass of tetrabutylammonium bromide (TBAB), 6.76 parts by mass of sodium iodide, and 490.0 parts by mass of xylene, and the mixture was heated to 50°C with stirring. Next, 253.2 parts by mass of a 48% by mass aqueous potassium hydroxide solution was slowly added dropwise while being careful of heat generation, and after completion of the addition, the temperature was raised to 60° C. and reacted for 10 hours. Next, 154.4 parts by mass of 2,6-xylenol was charged and reacted for 15 hours at 80° C. Next, 232.9 parts by mass of water was charged to dissolve the salt, and the lower layer was separated to remove the water layer, and the mixture was washed four times with 407.8 parts by mass of water. Subsequently, 213.2 parts by mass of 2,6-xylenol and 4.08 parts by mass of para-toluenesulfonic acid were charged, and the mixture was heated to 170° C. and reacted at the same temperature for 3 hours. After the reaction was completed, the mixture was cooled and neutralized with 3.19 parts by mass of 49% by mass sodium hydroxide, and the solvent and excess 2,6-xylenol were distilled off by heating under reduced pressure to obtain the target phenolic resin A-1 (hydroxyl group equivalent: 587 g / equivalent). The Mn of the phenolic resin A-1 was 1032 and the Mw was 1616. 13 C-NMR confirmed the quaternary carbon at the 9th position of fluorene. In addition, FD-MS confirmed the target product at m / z 466.3 and 766.4. The GPC chart of the obtained phenolic resin A-1 is shown in Figure 1. 13 The C-NMR chart is shown in Figure 2, and the FD-MS chart is shown in Figure 3.

[0132] <Synthesis of methacrylate-modified phenolic resin A-2> A flask equipped with a thermometer, a dropping funnel, a cooling tube, a fractionating tube, and a stirrer was charged with 100.0 parts by mass of phenolic resin A-1, 334.8 parts by mass of toluene, 1.04 parts by mass of 4-dimethylaminopyridine (DMAP), and 24.1 parts by mass of triethylamine (TEA), and 36.8 parts by mass of methacrylic anhydride were added dropwise. Next, the mixture was heated to 80°C while blowing in air, and reacted at the same temperature for 24 hours. After the reaction was completed, the organic layer was reprecipitated with methanol and dried to obtain methacrylate-modified phenolic resin A-2. The Mn of the obtained methacrylate-modified phenolic resin A-2 was 1135 and the Mw was 1895. The GPC chart of methacrylate-modified phenolic resin A-2 is shown in FIG. 4. 13 The C-NMR chart is shown in Figure 5, and the FD-MS chart is shown in Figure 6.

[0133] Example 2: Methacrylate-modified phenolic resin B-2 <Synthesis of phenolic resin B-1> A flask equipped with a thermometer, a dropping funnel, a condenser, a fractionating column, and a stirrer was charged with 130.0 parts by mass of fluorene, 205.4 parts by mass of α,α'-dichloro-p-xylene (PXDC), 7.56 parts by mass of TBAB, 10.6 parts by mass of sodium iodide, and 670.7 parts by mass of xylene, and the mixture was heated to 50°C with stirring. Next, 329.1 parts by mass of a 48% by mass aqueous potassium hydroxide solution was slowly added dropwise while taking care not to generate heat, and after completion of the addition, the temperature was raised to 60°C and reacted for 10 hours. Next, 173.4 parts by mass of 2,6-xylenol was charged, the temperature was raised to 80°C, and the reaction was carried out at the same temperature for 16 hours, after which 460.8 parts by mass of water was charged to dissolve the salt, the lower layer was separated to remove the aqueous layer, and the mixture was washed four times with 504.5 parts by mass of water. Subsequently, 169.2 parts by mass of 2,6-xylenol and 5.05 parts by mass of para-toluenesulfonic acid were charged, and the mixture was heated to 160° C. and reacted at the same temperature for 3 hours. After the reaction was completed, the mixture was cooled and neutralized with 2.19 parts by mass of 49% by mass sodium hydroxide, and the solvent and excess 2,6-xylenol were distilled off by heating under reduced pressure to obtain the target phenolic resin B-1 (hydroxyl group equivalent: 527 g / equivalent). The Mn of the phenolic resin B-1 was 1199, and the Mw was 1717. 13 C-NMR confirmed the quaternary carbon at the 9-position of fluorene. FD-MS confirmed the target product at m / z 614.4, 882.5, and 1106.6. The GPC chart of the obtained phenolic resin B-1 is shown in Figure 7. 13 The C-NMR chart is shown in Figure 8, and the FD-MS chart is shown in Figure 9.

[0134] <Synthesis of methacrylate-modified phenolic resin B-2> A flask equipped with a thermometer, a dropping funnel, a cooling tube, a fractionating tube, and a stirrer was charged with 100.0 parts by mass of phenolic resin B-1, 338.7 parts by mass of toluene, 1.16 parts by mass of DMAP, and 26.9 parts by mass of TEA, and 41.0 parts by mass of methacrylic anhydride were added dropwise. Next, the mixture was heated to 80°C while blowing air into it, and reacted at the same temperature for 24 hours. Next, the mixture was cooled to 40°C, washed 10 times with isopropyl alcohol (IPA) and water, and the organic layer was vacuum heated in a rotary evaporator to remove volatiles, and the phenolic resin B-1 was methacrylated to obtain a methacrylate-modified phenolic resin B-2. The Mn of the obtained methacrylate-modified phenolic resin B-2 was 1131, and the Mw was 1683. The GPC chart of the methacrylate-modified phenolic resin B-2 is shown in FIG. 13 The C-NMR chart is shown in Figure 11, and the FD-MS chart is shown in Figure 12.

[0135] Example 3: Methacrylate-modified phenolic resin C-2 <Synthesis of phenolic resin C-1> A flask equipped with a thermometer, a dropping funnel, a condenser, a fractionating column, and a stirrer was charged with 50.0 parts by mass of fluorene, 79.0 parts by mass of PXDC, 37.8 parts by mass of BCMB, 7.76 parts by mass of TBAB, 3.99 parts by mass of potassium iodide, and 333.5 parts by mass of xylene, and the mixture was heated to 50° C. with stirring. Next, 154.7 parts by mass of 48% by mass potassium hydroxide aqueous solution was slowly dropped while being careful of heat generation, and after the dropwise addition was completed, the temperature was raised to 60°C and reacted for 6 hours. Next, 91.1 parts by mass of 1-naphthol, 142.3 parts by mass of water, and 64.5 parts by mass of isopropyl alcohol were charged, the temperature was raised to 75°C, and the reaction was carried out at the same temperature for 5 hours, after which the lower layer was removed by liquid separation. 460.8 parts by mass of the obtained water was charged, the salt was dissolved, and the lower layer was separated to remove the water layer, and the mixture was washed six times with 209.6 parts by mass of water. Subsequently, 130.1 parts by mass of 1-naphthol and 4.19 parts by mass of para-toluenesulfonic acid were added, and the mixture was heated to 160° C. and reacted at the same temperature for 3 hours. After the reaction was completed, the mixture was cooled and neutralized with 1.82 parts by mass of 49% by mass sodium hydroxide, and the solvent and excess 1-naphthol were distilled off by heating under reduced pressure to obtain the target phenolic resin C-1 (hydroxyl group equivalent: 360 g / equivalent). The Mn of the phenolic resin C-1 was 782, and the Mw was 1277. 13 C-NMR confirmed the quaternary carbon at the 9-position of fluorene. FD-MS confirmed the target product at m / z 658.4, 734.4, 926.5, and 1002.6. The GPC chart of the obtained phenolic resin C-1 is shown in FIG. 13 The C-NMR chart is shown in Figure 14, and the FD-MS chart is shown in Figure 15.

[0136] <Synthesis of methacrylate modified phenolic resin C-2> A flask equipped with a thermometer, a dropping funnel, a cooling tube, a fractionating tube, and a stirrer was charged with 110.0 parts by mass of phenolic resin C-1, 333.0 parts by mass of toluene, 2.05 parts by mass of DMAP, and 0.13 parts by mass of butyl hydroxytoluene (BHT). After dehydration, 43.3 parts by mass of TEA was charged, and 66.0 parts by mass of methacrylic anhydride was added dropwise. Next, the mixture was heated to 80°C while blowing air into it, and reacted at the same temperature for 24 hours. Next, the mixture was cooled to 60°C, washed 10 times with IPA and water, and the organic layer was vacuum heated with a rotary evaporator to remove volatiles, and the phenolic resin C-1 was methacrylated to obtain a methacrylate-modified phenolic resin C-2. The Mn of the obtained methacrylate-modified phenolic resin C-2 was 932 and the Mw was 1533. The GPC chart of the methacrylate-modified phenolic resin C-2 is shown in FIG. 13 The C-NMR chart is shown in Figure 17, and the FD-MS chart is shown in Figure 18.

[0137] Example 4: Methacrylate-modified phenolic resin D-2 <Synthesis of phenolic resin D-1> A flask equipped with a thermometer, a dropping funnel, a condenser, a fractionating column, and a stirrer was charged with 100.0 parts by mass of fluorene, 158.0 parts by mass of PXDC, 14.6 parts by mass of TBAB, 6.76 parts by mass of sodium iodide, and 515.9 parts by mass of xylene, and the mixture was heated to 50° C. with stirring. Next, 253.2 parts by mass of a 48% by mass aqueous potassium hydroxide solution was slowly added dropwise while being careful not to generate heat, and after completion of the addition, the temperature was raised to 60° C. and reacted for 13.5 hours. Next, 136.6 parts by mass of ortho-cresol was charged, and the reaction was carried out at 60° C. for 30 hours and at 80° C. for a further 5 hours, after which 354.4 parts by mass of water and 31.2 parts by mass of an 85% aqueous phosphoric acid solution were charged while being careful not to generate heat, the salt was dissolved, the lower layer was separated to remove the aqueous layer, and the mixture was washed four times with 326.3 parts by mass of water. Subsequently, 130.1 parts by mass of ortho-cresol and 3.26 parts by mass of para-toluenesulfonic acid were added, and the mixture was heated to 160° C. and reacted at the same temperature for 4 hours. After the reaction was completed, the mixture was cooled and neutralized with 1.42 parts by mass of 49% by mass sodium hydroxide, and the solvent and excess ortho-cresol were distilled off by heating under reduced pressure to obtain the target phenolic resin D-1 (hydroxyl group equivalent: 452 g / equivalent). The Mn of the phenolic resin D-1 was 867 and the Mw was 1153. 13 C-NMR confirmed the quaternary carbon at the 9-position of fluorene. In addition, FD-MS confirmed the target product at m / z 586.3 and 854.5. The GPC chart of the obtained phenolic resin D-1 is shown in FIG. 13 The C-NMR chart is shown in Figure 20, and the FD-MS chart is shown in Figure 21.

[0138] <Synthesis of methacrylate-modified phenolic resin D-2> A flask equipped with a thermometer, a dropping funnel, a cooling tube, a fractionating tube, and a stirrer was charged with 100.0 parts by mass of phenolic resin D-1, 344.4 parts by mass of toluene, 1.35 parts by mass of DMAP, and 31.3 parts by mass of TEA, and 47.8 parts by mass of methacrylic anhydride were added dropwise. Next, the mixture was heated to 80°C while blowing air into it, and reacted at the same temperature for 24 hours. Next, the mixture was cooled to 40°C, washed 10 times with IPA and water, and the organic layer was vacuum heated in a rotary evaporator to remove volatiles, and the phenolic resin D-1 was methacrylated to obtain a methacrylate-modified phenolic resin D-2. The Mn of the obtained methacrylate-modified phenolic resin D-2 was 974, and the Mw was 1289. The GPC chart of the methacrylate-modified phenolic resin D-2 is shown in FIG. 13 The C-NMR chart is shown in Figure 23, and the FD-MS chart is shown in Figure 24.

[0139] Examples 5-8 and Comparative Example 1 The methacrylate-modified phenolic resin or terminal methacrylate-modified polyphenylene ether resin of Examples 1 to 4 ("SA9000-111" manufactured by Sabic Corporation) and divinylbenzene ("DVB-570" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., divinylbenzene purity 57%) were heated and mixed in the ratios shown in Table 1, and then poured into a mold that had been machined to a thickness of 2 mm and cured at 170°C for 30 minutes and at 200°C for 2 hours.

[0140] The physical properties of the cured products obtained as described above were evaluated as follows, and the results are shown in Table 1.

[0141] (1) Measurement of dielectric tangent In accordance with JIS-C-6481, the dielectric tangent of the test piece at 1 GHz and 10 GHz was measured using an impedance material analyzer "HP4291B" manufactured by Agilent Technologies Inc. after drying and storing it indoors at 23°C and 50% humidity for 24 hours. (2) Measurement of thermal expansion properties A thermomechanical analysis was performed in compression mode using a thermomechanical analyzer (TMA: Seiko Instruments "SS-6100") (measurement load: 88.8 mN, heating rate: 10°C / min twice, measurement temperature range: room temperature to 290°C). The thermal expansion coefficient from 40°C to 60°C in the second measurement was defined as α1, and the thermal expansion coefficient from 230°C to 250°C was defined as α2, to evaluate the thermal expansion properties.

[0142] [Table 1]

[0143] From the results shown in Table 1 above, it can be seen that cured products with excellent low dielectric tangents and low thermal expansion coefficients can be obtained by using the methacrylate-modified phenolic resins of Examples 1 to 4. In particular, it can be seen that when the methacrylate-modified phenolic resin of Example 3 is used, the cured product has an especially excellent low dielectric tangent and low thermal expansion coefficient in the high temperature range. [Industrial Applicability]

[0144] According to the present invention, it is possible to provide a (meth)acrylate-modified phenolic resin capable of achieving both a low dielectric tangent and a low thermal expansion coefficient at a high level, and also to provide a curable composition containing the resin and a cured product thereof. Furthermore, by using the curable composition or the cured product thereof, it is possible to provide a prepreg, a circuit board, a build-up film, a semiconductor encapsulant, and a semiconductor device that achieve both a low dielectric tangent and a low thermal expansion coefficient at a high level.

Claims

1. A (meth)acrylate-modified phenolic resin which is a (meth)acrylic acid ester of a reaction product of a fluorene compound (having no substituent at the 9-position), a phenolic hydroxyl group-containing compound, and a compound represented by general formula (1): 【Chemistry 1】 (where: Ar is Ar 1 -Y-Ar 1 Or Ar 1 and Ar 1 each independently represents an aromatic ring group which may have a substituent, Y is a single bond, an aliphatic hydrocarbon group having 1 to 6 carbon atoms, -P(=O)R a - group, an oxygen atom, a sulfur atom or a sulfonyl group, and R a is an aromatic ring group, R 1 each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 4 carbon atoms, X is a leaving group.

2. The (meth)acrylate modified phenolic resin according to claim 1, wherein the fluorene compound is 0.01 to 0.99 moles per mole of the compound represented by the general formula (1).

3. A (meth)acrylate-modified phenolic resin represented by general formula (15): 【Chemistry 2】 (where: Z is independently a group represented by general formula (12A): 【Chemistry 3】 or a structural unit represented by general formula (13A): 【Chemistry 4】 It is a structural unit represented by Z' is independently a group represented by general formula (12A'): 【Chemistry 5】 or a structural unit represented by general formula (13A'): 【Chemistry 6】 It is a structural unit represented by Ar is independently Ar 1 Or Ar 1 -Y-Ar 1 and Ar 1 each independently represents an aromatic ring group which may have a substituent, Y is a single bond, an aliphatic hydrocarbon group having 1 to 6 carbon atoms, -P(=O)R a - group, an oxygen atom, a sulfur atom or a sulfonyl group, and R a is an aromatic ring group, R 1 each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 4 carbon atoms, R 2 each independently represents an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, m is independently an integer from 0 to 4; R b are each independently a hydrogen atom or a methyl group, R 3 are each independently an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, or two R 3 may form a ring together with the carbon atom to which they are attached, n is independently an integer from 0 to 3; R 2’ each independently represents an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, m' is independently an integer from 0 to 4; R b’ are each independently a hydrogen atom or a methyl group, R 3’ are each independently an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, or two R 3’ may form a ring together with the carbon atom to which they are attached, Each n' is independently an integer from 0 to 4; p is an average value and is a number greater than 0; however, The resin contains a structural unit represented by general formula (12A) and / or general formula (12A') and a structural unit represented by general formula (13A) and / or general formula (13A').

4. The (meth)acrylate-modified phenolic resin according to claim 3, comprising at least one of a compound represented by general formula (15-1) and a compound represented by general formula (15-2): 【Chemistry 7】 (where: Ar, Z, R 1 , R b’ , R 3’ and n' have the same meaning as in claim 3.

5. The (meth)acrylate modified phenolic resin according to claim 1 or 3, having a vinyl equivalent of 100 to 10,000.

6. The (meth)acrylate-modified phenolic resin according to claim 1 or 3, having a number average molecular weight of 100 to 10,000.

7. A curable composition comprising the (meth)acrylate-modified phenolic resin according to claim 1 or 3.

8. A cured product of the curable composition according to claim 7.

9. A prepreg comprising a reinforcing substrate and a semi-cured product of the curable composition according to claim 7 impregnated into the reinforcing substrate.

10. A circuit board which is a laminate of the prepreg according to claim 9 and copper foil.

11. A build-up film comprising the curable composition according to claim 7.

12. A semiconductor encapsulant comprising the curable composition according to claim 7.

13. A semiconductor device comprising the cured product of the semiconductor encapsulation material according to claim 12.

Citation Information

Cited By

  • Resin compositions, cured products, prepregs, resin composites, printed circuit boards, and semiconductor devices

    CN123125250A