Optical laminate and display system

The optical laminate addresses bubble defects in VR goggles by incorporating a high-modulus support layer and strategically placed adhesive layers, enhancing image quality and structural integrity.

WO2024203349A1PCT designated stage expired Publication Date: 2024-10-03NITTO DENKO CORP
View PDF 20 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/009850
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-13
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional optical laminates used in image display devices, such as VR goggles, suffer from defects like bubbles that affect image quality due to irregularities during the lamination process.

Method used

An optical laminate design featuring a polarizing member with an absorbing polarizing film, a protective layer, and a support layer with an indentation modulus of 1 GPa or more, along with adhesive layers directly adjacent to the support layer, to suppress defects like bubbles by ensuring smooth lamination and minimizing surface irregularities.

Benefits of technology

The proposed optical laminate effectively reduces bubble formation and enhances image display performance by integrating a support layer with high indentation modulus and strategically positioned adhesive layers, improving the structural integrity and optical clarity of the laminate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024009850_03102024_PF_FP_ABST
    Figure JP2024009850_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides an optical laminate in which defects are suppressed. An optical laminate according to the present invention comprises: a polarizing member having an absorption-type polarizing film and a protective layer disposed on at least one side of the absorption-type polarizing film; and a first phase difference member. The optical laminate further comprises a support layer having a push-in elastic modulus of 1 GPa or higher. An adhesive layer is disposed directly adjacent to the support layer.
Need to check novelty before this filing date? Find Prior Art

Description

Optical laminate and display system

[0001] The present invention relates to an optical stack and a display system.

[0002] Image display devices, such as liquid crystal display devices and electroluminescence (EL) display devices (e.g., organic EL display devices), are rapidly becoming popular. In image display devices, optical components such as polarizing components and phase difference components are generally used to realize image display and improve image display performance (see, for example, Patent Document 1).

[0003] In recent years, new applications of image display devices have been developed. For example, goggles with displays (VR goggles) for realizing virtual reality (VR) have begun to be commercialized. In VR goggles, the display is enlarged for viewing by a viewer, and therefore, in an optical laminate applied to VR goggles, even small defects that are acceptable in optical laminates applied to conventional image display devices may become problematic.

[0004] Japanese Patent Application Laid-Open No. 2021-103286

[0005] An object of the present invention is to provide an optical laminate in which defects are suppressed.

[0006] [1] According to one aspect of the present invention, there is provided an optical laminate including a polarizing member having an absorptive polarizing film and a protective layer disposed on at least one side thereof, and a first phase difference member, wherein the optical laminate further includes a support layer having an indentation modulus of 1 GPa or more, and an adhesive layer disposed directly adjacent to the support layer. [2] The optical laminate described in [1] above may include, in this order, a surface adhesive layer, the polarizing member, a first adhesive layer, the first phase difference member, a second adhesive layer, and a protective member. [3] In the optical laminate described in [2] above, at least one selected from the surface adhesive layer, the first adhesive layer, and the second adhesive layer may be disposed directly adjacent to the support layer. [4] The optical laminate described in [1] above may include, in this order, a surface adhesive layer, a second phase difference member, a third adhesive layer, the polarizing member, the first adhesive layer, the first phase difference member, a second adhesive layer, and a protective member. [5] In the optical laminate according to [4] above, at least one selected from the surface adhesive layer, the first adhesive layer, the second adhesive layer, and the third adhesive layer may be disposed directly adjacent to the support layer. [6] In the optical laminate according to any one of [1] to [5] above, the support layer may be a hard coat layer. [7] In the optical laminate according to any one of [1] to [6] above, the thickness of the support layer may be 0.5 μm to 15 μm. [8] In the optical laminate according to any one of [1] to [7] above, the support layer may be disposed directly adjacent to the polarizing member on the side opposite to the side on which the first phase difference member is disposed. [9] In the optical laminate according to any one of [1] to [8] above, the elastic modulus of the adhesive layer disposed directly adjacent to the support layer may be 0.01 MPa to 1 MPa.

[10] According to another aspect of the present invention, there is provided a display system including the optical laminate according to any one of [1] to [9] above.

[0007] According to an embodiment of the present invention, an optical laminate in which defects such as bubbles are suppressed can be provided.

[0008] 1 is a schematic diagram showing a schematic configuration of a display system of VR goggles according to one embodiment of the present invention; 2 is a schematic cross-sectional view showing a schematic configuration of an optical laminate according to one embodiment of the present invention; 3 is a schematic cross-sectional view showing a schematic configuration of an optical laminate according to one embodiment of the present invention;

[0009] Hereinafter, embodiments of the present invention will be described with reference to the drawings, but the present invention is not limited to these embodiments. In order to clarify the description, the drawings may schematically show the width, thickness, shape, etc. of each part compared to the embodiments, but these are merely examples and do not limit the interpretation of the present invention. Furthermore, in the drawings, the same or equivalent elements are given the same reference numerals, and redundant explanations may be omitted.

[0010] (Definition of Terms and Symbols) The definitions of terms and symbols used in this specification are as follows. (1) Refractive Index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the in-plane direction perpendicular to the slow axis (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-Plane Retardation (Re) "Re(λ)" is the in-plane retardation measured with light having a wavelength of λ nm at 23°C. For example, "Re(550)" is the in-plane retardation measured with light having a wavelength of 550 nm at 23°C. Re(λ) is calculated by the formula: Re(λ) = (nx - ny) × d, where d (nm) is the thickness of the layer (film). (3) Thickness Direction Retardation (Rth) "Rth(λ)" is the retardation in the thickness direction measured with light having a wavelength of λ nm at 23°C. For example, "Rth(550)" refers to the retardation in the thickness direction measured with light having a wavelength of 550 nm at 23°C. Rth(λ) is calculated by the formula: Rth(λ) = (nx - nz) × d, where d (nm) is the thickness of the layer (film). (4) Nz Coefficient The Nz coefficient is calculated by Nz = Rth / Re. (5) Angle When angles are referred to in this specification, they include both clockwise and counterclockwise angles relative to a reference direction. Thus, for example, "45°" means ±45°. Furthermore, in this specification, "substantially parallel" includes angles within a range of 0° ±10°, such as 0° ±5°, preferably 0° ±3°, and more preferably 0° ±1°. "Substantially perpendicular" includes angles within a range of 90° ±10°, such as 90° ±5°, preferably 90° ±3°, and more preferably 90° ±1°.

[0011] A. Display System FIG. 1 is a schematic diagram showing the overall configuration of a display system according to one embodiment of the present invention. FIG. 1 schematically illustrates the arrangement and shape of each component of a display system 2. The display system 2 includes a display element 12, a reflective polarizing element 14, a first lens unit 16, a half mirror 18, a first phase difference element 20, a lens portion phase difference element 22, and a second lens unit 24. The reflective polarizing element 14 is disposed in front of the display surface 12a of the display element 12 and can reflect light emitted from the display element 12. The first lens unit 16 is disposed on the optical path between the display element 12 and the reflective polarizing element 14, and the half mirror 18 is disposed between the display element 12 and the first lens unit 16. The first phase difference element 20 is disposed on the optical path between the display element 12 and the half mirror 18, and the lens portion phase difference element 22 is disposed on the optical path between the half mirror 18 and the reflective polarizing element 14.

[0012] The components arranged in front of the half mirror (in the illustrated example, the half mirror 18, the first lens section 16, the lens section phase difference member 22, the reflective polarizing member 14, and the second lens section 24) may be collectively referred to as the lens section (lens section 4).

[0013] The display element 12 is, for example, a liquid crystal display or an organic EL display, and has a display surface 12 a for displaying an image. The light emitted from the display surface 12 a passes through, for example, a polarizing member (typically, a polarizing film) that may be included in the display element 12, and is converted into first linearly polarized light.

[0014] The first phase difference member 20 includes a first λ / 4 member that can convert first linearly polarized light incident on the first phase difference member 20 into first circularly polarized light. When the first phase difference member does not include any member other than the first λ / 4 member, the first phase difference member may correspond to the first λ / 4 member. The first phase difference member 20 may be provided integrally with the display element 12.

[0015] The half mirror 18 transmits the light emitted from the display element 12 and reflects the light reflected by the reflective polarizing member 14 back toward the reflective polarizing member 14. The half mirror 18 is provided integrally with the first lens portion 16.

[0016] The lens portion phase difference member 22 includes a second λ / 4 member that can transmit light reflected by the reflective polarizing member 14 and the half mirror 18 through the reflective polarizing member 14. When the lens portion phase difference member does not include any member other than the second λ / 4 member, the lens portion phase difference member can correspond to the second λ / 4 member. The lens portion phase difference member 22 may be provided integrally with the first lens portion 16.

[0017] The first circularly polarized light emitted from the first λ / 4 element included in the first phase difference element 20 passes through the half mirror 18 and the first lens portion 16, and is converted into the second linearly polarized light by the second λ / 4 element included in the lens portion phase difference element 22. The second linearly polarized light emitted from the second λ / 4 element is reflected toward the half mirror 18 without passing through the reflective polarizing element 14. At this time, the polarization direction of the second linearly polarized light incident on the reflective polarizing element 14 is the same as the reflection axis of the reflective polarizing element 14. Therefore, the second linearly polarized light incident on the reflective polarizing element 14 is reflected by the reflective polarizing element 14.

[0018] The second linearly polarized light reflected by the reflective polarizing element 14 is converted into second circularly polarized light by the second λ / 4 element included in the lens portion phase difference element 22, and the second circularly polarized light output from the second λ / 4 element passes through the first lens portion 16 and is reflected by the half mirror 18. The second circularly polarized light reflected by the half mirror 18 passes through the first lens portion 16 and is converted into third linearly polarized light by the second λ / 4 element included in the lens portion phase difference element 22. The third linearly polarized light is transmitted through the reflective polarizing element 14. At this time, the polarization direction of the third linearly polarized light incident on the reflective polarizing element 14 is the same as the transmission axis of the reflective polarizing element 14. Therefore, the third linearly polarized light incident on the reflective polarizing element 14 is transmitted through the reflective polarizing element 14.

[0019] The light transmitted through the reflective polarizing member 14 passes through the second lens portion 24 and enters the user's eye 26 .

[0020] Although not shown, the display system 2 may also include an absorptive polarizing element disposed in front of the reflective polarizing element 14. The reflection axis of the reflective polarizing element and the absorption axis of the absorptive polarizing element may be disposed approximately parallel to each other, and the transmission axis of the reflective polarizing element and the transmission axis of the absorptive polarizing element may be disposed approximately parallel to each other. This allows the third linearly polarized light that has passed through the reflective polarizing element 14 to pass directly through the absorptive polarizing element.

[0021] The above describes the progression of light from when it is emitted from the display element 12 to when it enters the user's eye 26 in the display system 2. However, a portion of the light (not shown) that is emitted from the display element 12 and enters the half mirror 18 may be reflected by the half mirror 18, and a portion of the light (not shown) that is reflected by the reflective polarizing element 14 and enters the half mirror 18 may be transmitted through the half mirror 18.

[0022] For example, the absorption axis of the polarizing member included in the display element 12 and the reflection axis of the reflective polarizing member 14 may be disposed approximately parallel to each other or approximately perpendicular to each other. The angle formed between the absorption axis of the polarizing member included in the display element 12 and the slow axis of the first λ / 4 member included in the first retardation member 20 is, for example, 40° to 50°, may be 42° to 48°, or may be approximately 45°. The angle formed between the absorption axis of the polarizing member included in the display element 12 and the slow axis of the second λ / 4 member included in the lens portion retardation member 22 is, for example, 40° to 50°, may be 42° to 48°, or may be approximately 45°.

[0023] The in-plane retardation Re(550) of the first λ / 4 component is, for example, 100 nm to 190 nm, or may be 110 nm to 180 nm, 130 nm to 160 nm, or 135 nm to 155 nm. The first λ / 4 component preferably exhibits an inverse dispersion wavelength characteristic in which the retardation value increases according to the wavelength of the measurement light. The first λ / 4 component preferably satisfies the relationship Re(450)<Re(550)<Re(650). The Re(450) / Re(550) of the first λ / 4 component may be, for example, 0.75 or more and less than 1, or 0.8 or more and 0.95 or less.

[0024] The in-plane retardation Re(550) of the second λ / 4 component is, for example, 100 nm to 190 nm, or may be 110 nm to 180 nm, 130 nm to 160 nm, or 135 nm to 155 nm. The second λ / 4 component preferably exhibits an inverse dispersion wavelength characteristic in which the retardation value increases according to the wavelength of the measurement light. The second λ / 4 component preferably satisfies the relationship Re(450)<Re(550)<Re(650). The Re(450) / Re(550) of the second λ / 4 component may be, for example, 0.75 or more and less than 1, or 0.8 or more and 0.95 or less.

[0025] B. Optical Laminate An optical laminate according to an embodiment of the present invention may include, for example, the optical element provided in the display system described in Section A, and may be included in the display system as a component of the display system. Specifically, an optical laminate according to an embodiment of the present invention includes a polarizing element having an absorptive polarizing film and a protective layer disposed on at least one side of the polarizing element, and a first retardation element. The optical laminate according to an embodiment of the present invention may also include an adhesive layer for integrating the components constituting the optical laminate and / or an adhesive layer (also referred to as a "surface adhesive layer") for bonding the optical laminate to another component. The optical laminate according to an embodiment of the present invention further includes a support layer having a predetermined indentation elastic modulus, and the adhesive layer is disposed directly adjacent to the support layer. Note that, in this specification, "directly adjacent" means directly adjacent without an adhesive layer interposed therebetween. Note that, in this specification, the term "adjacent" simply refers not only to being directly adjacent without an adhesive layer interposed therebetween, but also to being adjacent via an adhesive layer.

[0026] The production of the optical laminate may involve laminating an adhesive layer to a component, which may result in small bubbles forming at the interface and causing defects. In contrast, according to an embodiment of the present invention, the adhesive layer is disposed directly adjacent to the support layer, thereby suppressing the problem of bubbles. The reason for this effect is presumed to be as follows, without limiting the present invention in any way. That is, if the surface of the component to be laminated is uneven when laminating the adhesive layer, bubbles may form due to the unevenness. However, by providing a support layer having a predetermined indentation elastic modulus and laminating the adhesive layer on the support layer, the generation of such bubbles can be suppressed.

[0027] 2 is a schematic cross-sectional view showing the general configuration of an optical laminate according to one embodiment of the present invention. The optical laminate 100A includes, in this order, a surface adhesive layer 42, a polarizing member 10, a first adhesive layer 44, a first retardation member 20, a second adhesive layer 46, and a protective member 30. In the optical laminate 100A, a support layer 50 is provided directly adjacent to the surface adhesive layer 42 side of the polarizing member 10, and the surface adhesive layer 42 is disposed directly adjacent to the support layer 50. The polarizing member 10 may correspond to a polarizing member that may be included in the display element 12 of the display system 2. The first retardation member 20 includes a first λ / 4 member 20a and may correspond to the first retardation member 20 of the display system 2. For example, when the display element 12 is a liquid crystal display, the optical laminate 100A can be attached to the front (viewing side) of the liquid crystal cell via the surface adhesive layer 42, so that the polarizing element 10 can be used as the viewing side polarizing element of a liquid crystal panel that includes a back side polarizing element, a liquid crystal cell, and a viewing side polarizing element in that order.

[0028] FIG. 3 is a schematic cross-sectional view showing the general configuration of an optical laminate according to one embodiment of the present invention. The optical laminate 100B includes, in this order, a surface adhesive layer 42, a second retardation member 60, a third adhesive layer 48, a polarizing member 10, a first adhesive layer 44, a first retardation member 20, a second adhesive layer 46, and a protective member 30. In the optical laminate 100B, a support layer 50 is provided directly adjacent to the third adhesive layer 48 side of the polarizing member 10, and the third adhesive layer 48 is disposed directly adjacent to the support layer 50. The polarizing member 10 may correspond to a polarizing member that may be included in the display element 12 of the display system 2. The first retardation member 20 includes a first λ / 4 member 20a and may correspond to the first retardation member 20 of the display system 2. The second retardation member 60 may correspond to a retardation member that may be included in the display element 12. For example, the second phase difference member 60 includes a λ / 4 member (also referred to as a "third λ / 4 member") 60a. The angle between the absorption axis of the polarizing member 10 and the slow axis of the third λ / 4 member is, for example, 40° to 50°, or may be 42° to 48°, or may be approximately 45°. When the display element 12 is an organic EL display, providing the third λ / 4 member together with the polarizing member 10 in front of (on the viewing side of) the organic EL panel can solve problems such as external light reflection and background glare that may be caused by a metal layer included in the organic EL display. When the second phase difference member 60 does not include any member other than the third λ / 4 member, the second phase difference member 60 can correspond to the third λ / 4 member.

[0029] 2 and 3, the first phase difference member 20 may include, in addition to the first λ / 4 member 20a, a member whose refractive index characteristics satisfy the relationship nz > nx = ny (hereinafter also referred to as a "first positive C plate"). In this case, in the first phase difference member 20, it is preferable that the first λ / 4 member 20a is located closer to the polarizing member 10 than the first positive C plate. The first λ / 4 member 20a and the first positive C plate can be laminated typically via an adhesive layer.

[0030] 3, the second phase difference member 60 may include, in addition to the third λ / 4 member 60a, a member whose refractive index characteristics satisfy the relationship nz > nx = ny (hereinafter also referred to as a "second positive C plate") The third λ / 4 member 60a and the second positive C plate may be laminated typically via an adhesive layer.

[0031] <Polarizing Member> The polarizing member 10 has an absorptive polarizing film 10a, a display element-side protective layer 10b arranged on the side opposite to the side on which the first retardation member 20 is arranged, and a lens unit-side protective layer 10c arranged on the side on which the first retardation member 20 is arranged. Either the display element-side protective layer 10b or the lens unit-side protective layer 10c may be omitted depending on the purpose. Preferably, the polarizing member has an absorptive polarizing film 10a and a display element-side protective layer 10b.

[0032] The absorptive polarizing film is made of, for example, a resin film containing a dichroic material. The thickness of the absorptive polarizing film is, for example, 1 μm to 20 μm, or may be 2 μm to 15 μm, or may be 12 μm or less, 10 μm or less, 8 μm or less, or may be 5 μm or less.

[0033] The absorptive polarizing film may be made from a single layer of resin film or may be made from a laminate of two or more layers.

[0034] When the absorptive polarizing film is produced from a single-layer resin film, for example, an absorptive polarizing film can be obtained by subjecting a hydrophilic polymer film such as a polyvinyl alcohol (PVA)-based film, a partially formalized PVA-based film, or a partially saponified ethylene-vinyl acetate copolymer-based film to a dyeing treatment with iodine or a dichroic substance such as a dichroic dye, a stretching treatment, etc. Among these, an absorptive polarizing film obtained by dyeing a PVA-based film with iodine and uniaxially stretching it is preferred.

[0035] The dyeing with iodine is carried out, for example, by immersing the PVA-based film in an aqueous iodine solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. The stretching may be carried out after the dyeing treatment or while dyeing. Alternatively, the PVA-based film may be dyed after stretching. If necessary, the PVA-based film may be subjected to a swelling treatment, a crosslinking treatment, a washing treatment, a drying treatment, or the like.

[0036] Examples of laminates produced using the two or more layer laminate include a laminate of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, and a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate. An absorptive polarizing film obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate can be produced, for example, by applying a PVA-based resin solution to the resin substrate and drying the solution to form a PVA-based resin layer on the resin substrate, thereby obtaining a laminate of the resin substrate and the PVA-based resin layer, and then stretching and dyeing the laminate to convert the PVA-based resin layer into an absorptive polarizing film. In this embodiment, a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin is preferably formed on one side of the resin substrate. The stretching typically involves immersing the laminate in an aqueous boric acid solution to stretch it. Furthermore, the stretching may further include in-air stretching of the laminate at a high temperature (e.g., 95°C or higher) before stretching in the boric acid aqueous solution, as necessary. In addition, in this embodiment, the laminate is preferably subjected to a drying shrinkage treatment in which the laminate is heated while being transported in the longitudinal direction, thereby shrinking the laminate by 2% or more in the width direction. Typically, the manufacturing method of this embodiment includes subjecting the laminate to an auxiliary in-air stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment, in this order. By introducing auxiliary stretching, it is possible to increase the crystallinity of the PVA, even when the PVA is coated on a thermoplastic resin, thereby achieving high optical properties. Furthermore, by simultaneously increasing the orientation of the PVA in advance, problems such as a decrease in orientation or dissolution of the PVA when immersed in water in the subsequent dyeing or stretching steps can be prevented, thereby achieving high optical properties. Furthermore, when the PVA-based resin layer is immersed in a liquid, the disordering of the polyvinyl alcohol molecules and the decrease in orientation can be suppressed compared to when the PVA-based resin layer does not contain a halide. This can improve the optical properties of the absorptive polarizing film obtained through treatment steps in which the laminate is immersed in a liquid, such as a dyeing treatment and an underwater stretching treatment.Furthermore, the optical properties can be improved by shrinking the laminate in the width direction through a drying shrinkage treatment.The obtained resin substrate / absorptive polarizing film laminate may be used as is (i.e., the resin substrate may be used as a protective layer for the absorptive polarizing film), or any suitable protective layer may be laminated depending on the purpose on the surface obtained by peeling the resin substrate from the resin substrate / absorptive polarizing film laminate or on the surface opposite to the peeled surface. Details of such methods for producing an absorptive polarizing film are described in, for example, JP-A-2012-73580 and Japanese Patent No. 6,470,455. The entire disclosures of these publications are incorporated herein by reference.

[0037] The display element-side protective layer and the lens unit-side protective layer are each composed of any suitable film that can be used as a protective layer for an absorptive polarizing film. Examples of materials that can be used to form the protective layer include cellulose-based resins such as triacetyl cellulose (TAC), cycloolefin-based resins such as polynorbornene, (meth)acrylic resins, polyester-based resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyolefin-based resins such as polyethylene, and polycarbonate-based resins. Representative examples of (meth)acrylic resins include (meth)acrylic resins having a lactone ring structure. Examples of (meth)acrylic resins having a lactone ring structure are described in, for example, JP 2000-230016 A, JP 2001-151814 A, JP 2002-120326 A, JP 2002-254544 A, and JP 2005-146084 A. These publications are incorporated herein by reference.

[0038] The thickness of the protective layer is, for example, 10 μm to 80 μm, preferably 15 μm to 70 μm, and more preferably 20 μm to 50 μm.

[0039] The crossed transmittance (Tc) of the absorptive polarizing element (absorptive polarizing film) is preferably 0.5% or less, more preferably 0.1% or less, and even more preferably 0.05% or less. The single transmittance (Ts) of the absorptive polarizing element (absorptive polarizing film) is, for example, 41.0% to 45.0%, and preferably 42.0% or more. The polarization degree (P) of the absorptive polarizing element (absorptive polarizing film) is, for example, 99.0% to 99.997%, and preferably 99.9% or more.

[0040] <First λ / 4 Member> The in-plane retardation Re(550) and wavelength dispersion characteristics of the retardation value of the first λ / 4 member 20a are as described in Section A. In addition, in the optical laminate, the angle between the slow axis of the first λ / 4 member and the absorption axis of the polarizing member is, for example, 40° to 50°, or may be 42° to 48°, or may be approximately 45°.

[0041] The first λ / 4 member preferably has a refractive index characteristic that satisfies the relationship nx>ny≧nz. Here, "ny=nz" includes not only the case where ny and nz are completely equal, but also the case where they are substantially equal. Therefore, there may be cases where ny<nz. The Nz coefficient of the first λ / 4 member is preferably 0.9 to 3, more preferably 0.9 to 2.5, even more preferably 0.9 to 1.5, and particularly preferably 0.9 to 1.3.

[0042] The first λ / 4 member may be made of any suitable material that satisfies the above-mentioned characteristics, and may be, for example, a stretched resin film or an oriented and solidified layer of a liquid crystal compound.

[0043] Examples of resins contained in the resin film include polycarbonate-based resins, polyester carbonate-based resins, polyester-based resins, polyvinyl acetal-based resins, polyarylate-based resins, cyclic olefin-based resins, cellulose-based resins, polyvinyl alcohol-based resins, polyamide-based resins, polyimide-based resins, polyether-based resins, polystyrene-based resins, and acrylic-based resins. These resins may be used alone or in combination. Examples of methods for combining include blending and copolymerization. When the first λ / 4 member exhibits reverse dispersion wavelength characteristics, a resin film containing a polycarbonate-based resin or a polyester carbonate-based resin (hereinafter sometimes simply referred to as a polycarbonate-based resin) can be suitably used.

[0044] Any suitable polycarbonate resin can be used as the polycarbonate resin. For example, the polycarbonate resin contains structural units derived from a fluorene-based dihydroxy compound, structural units derived from an isosorbide-based dihydroxy compound, and structural units derived from at least one dihydroxy compound selected from the group consisting of alicyclic diols, alicyclic dimethanols, di-, tri-, or polyethylene glycols, and alkylene glycols or spiroglycols. Preferably, the polycarbonate resin contains structural units derived from a fluorene-based dihydroxy compound, structural units derived from an isosorbide-based dihydroxy compound, structural units derived from an alicyclic dimethanol and / or structural units derived from di-, tri-, or polyethylene glycol; more preferably, it contains structural units derived from a fluorene-based dihydroxy compound, structural units derived from an isosorbide-based dihydroxy compound, and structural units derived from di-, tri-, or polyethylene glycol. The polycarbonate resin may contain structural units derived from other dihydroxy compounds as needed. Details of polycarbonate-based resins that can be suitably used for the first λ / 4 member and methods for forming the first λ / 4 member are described, for example, in JP 2014-10291 A, JP 2014-26266 A, JP 2015-212816 A, JP 2015-212817 A, and JP 2015-212818 A, and the descriptions in these publications are incorporated herein by reference.

[0045] The thickness of the first λ / 4 member made of a stretched resin film is, for example, 10 μm to 100 μm, preferably 10 μm to 70 μm, and more preferably 20 μm to 60 μm.

[0046] The above-mentioned liquid crystal compound alignment solidified layer is a layer in which the liquid crystal compound is aligned in a predetermined direction within the layer and the alignment state is fixed. The term "alignment solidified layer" encompasses an alignment solidified layer obtained by curing a liquid crystal monomer, as described below. In the first λ / 4 member, typically, rod-shaped liquid crystal compounds are aligned in the slow axis direction of the first λ / 4 member (homogeneous alignment). Examples of rod-shaped liquid crystal compounds include liquid crystal polymers and liquid crystal monomers. The liquid crystal compound is preferably polymerizable. If the liquid crystal compound is polymerizable, the alignment state of the liquid crystal compound can be fixed by aligning the liquid crystal compound and then polymerizing it.

[0047] The alignment and solidification layer of the liquid crystal compound (liquid crystal alignment and solidification layer) can be formed by performing an alignment treatment on the surface of a predetermined substrate, applying a coating liquid containing a liquid crystal compound to the surface to align the liquid crystal compound in a direction corresponding to the alignment treatment, and fixing the alignment state. Any appropriate alignment treatment can be used as the alignment treatment. Specific examples include mechanical alignment treatment, physical alignment treatment, and chemical alignment treatment. Specific examples of mechanical alignment treatment include rubbing treatment and stretching treatment. Specific examples of physical alignment treatment include magnetic field alignment treatment and electric field alignment treatment. Specific examples of chemical alignment treatment include oblique vapor deposition and photoalignment treatment. Any appropriate treatment conditions can be used for the various alignment treatments depending on the purpose.

[0048] The alignment of liquid crystal compounds is achieved by treating them at a temperature at which they exhibit a liquid crystal phase depending on the type of liquid crystal compound. By performing such temperature treatment, the liquid crystal compounds assume a liquid crystal state and are aligned in accordance with the alignment treatment direction on the substrate surface.

[0049] In one embodiment, the alignment state is fixed by cooling the liquid crystal compound aligned as described above. When the liquid crystal compound is polymerizable or crosslinkable, the alignment state is fixed by subjecting the liquid crystal compound aligned as described above to a polymerization treatment or a crosslinking treatment.

[0050] Any suitable liquid crystal polymer and / or liquid crystal monomer can be used as the liquid crystal compound. The liquid crystal polymer and the liquid crystal monomer can be used alone or in combination. Specific examples of liquid crystal compounds and methods for producing a liquid crystal alignment solidified layer are described in, for example, JP 2006-163343 A, JP 2006-178389 A, and WO 2018 / 123551 A. The descriptions in these publications are incorporated herein by reference.

[0051] The thickness of the first λ / 4 member formed of the liquid crystal alignment solidified layer is, for example, 1 μm to 10 μm, preferably 1 μm to 8 μm, more preferably 1 μm to 6 μm, and even more preferably 1 μm to 4 μm.

[0052] <First Positive C Plate> The thickness direction retardation Rth(550) of the first positive C plate is preferably −20 nm to −200 nm, more preferably −30 nm to −180 nm, even more preferably −40 nm to −160 nm, and particularly preferably −50 nm to −140 nm. Here, "nx=ny" encompasses not only the case where nx and ny are strictly equal, but also the case where nx and ny are substantially equal. The in-plane retardation Re(550) of the first positive C plate is, for example, less than 10 nm.

[0053] The first positive C plate can be formed of any suitable material, but is preferably composed of a film containing a liquid crystal material fixed in homeotropic alignment. The liquid crystal material (liquid crystal compound) that can be homeotropically aligned may be a liquid crystal monomer or a liquid crystal polymer. Specific examples of such liquid crystal compounds and methods for forming a positive C plate include the liquid crystal compounds and methods for forming the retardation layer described in paragraphs

[0020] to

[0028] of JP 2002-333642 A. In this case, the thickness of the first positive C plate is preferably 0.5 μm to 5 μm.

[0054] <Third λ / 4 Member> The in-plane retardation Re(550) of the third λ / 4 member 60a is, for example, 100 nm to 190 nm, but may also be 110 nm to 180 nm, 130 nm to 160 nm, or 135 nm to 155 nm. The third λ / 4 member preferably exhibits an inverse dispersion wavelength characteristic in which the retardation value increases according to the wavelength of the measurement light. The Re(450) / Re(550) of the third λ / 4 member may be, for example, 0.75 or more and less than 1, or 0.8 or more and 0.95 or less. The third λ / 4 member preferably exhibits a refractive index characteristic of nx > ny ≧ nz. The Nz coefficient of the third λ / 4 member is preferably 0.9 to 3, more preferably 0.9 to 2.5, even more preferably 0.9 to 1.5, and particularly preferably 0.9 to 1.3.

[0055] The third λ / 4 member is formed of any appropriate material that can satisfy the above characteristics. The third λ / 4 member may be, for example, a stretched resin film or an oriented and solidified layer of a liquid crystal compound. The same explanation as for the first λ / 4 member can be applied to a third λ / 4 member formed of a stretched resin film or an oriented and solidified layer of a liquid crystal compound. The first λ / 4 member and the third λ / 4 member may be members having the same configuration (e.g., forming material, thickness, optical properties, etc.) or may be members having different configurations.

[0056] <Second Positive C Plate> The thickness direction retardation Rth(550) of the second positive C plate is preferably −20 nm to −200 nm, more preferably −30 nm to −180 nm, even more preferably −40 nm to −160 nm, and particularly preferably −50 nm to −140 nm. Here, "nx=ny" encompasses not only the case where nx and ny are strictly equal, but also the case where nx and ny are substantially equal. The in-plane retardation Re(550) of the second positive C plate is, for example, less than 10 nm.

[0057] The second positive C plate may be formed of any suitable material, but is preferably composed of a film containing a liquid crystal material fixed in a homeotropic alignment. The same explanations as for the first positive C plate can be applied to the materials and methods for forming such a second positive C plate. The first positive C plate and the second positive C plate may be made of components having the same configuration (e.g., forming material, thickness, optical properties, etc.) or different configurations.

[0058] <Protective Member> The protective member 30 typically includes a substrate. The substrate may be composed of any appropriate film. Examples of materials that form the main component of the film constituting the substrate include cellulose-based resins such as triacetyl cellulose (TAC), polyester-based, polyvinyl alcohol-based, polycarbonate-based, polyamide-based, polyimide-based, polyethersulfone-based, polysulfone-based, polystyrene-based, cycloolefin-based resins such as polynorbornene, polyolefin-based, (meth)acrylic, and acetate-based resins. The thickness of the substrate is preferably 5 μm to 80 μm, more preferably 10 μm to 50 μm, and even more preferably 15 μm to 40 μm.

[0059] The protective member 30 is preferably a laminated film having a substrate and a surface treatment layer. A protective member having a surface treatment layer can be disposed so that the substrate is located on the first retardation member 20 side. The thickness of the surface treatment layer is, for example, 0.5 μm to 10 μm, or may be 1 μm to 7 μm, or may be 2 μm to 5 μm. The surface treatment layer can have any appropriate function. For example, the surface treatment layer preferably has an anti-reflection function.

[0060] <Adhesive Layer> Typically, an adhesive layer or a pressure-sensitive adhesive layer is used as the adhesive layer. The surface adhesive layer for bonding the optical laminate itself to another member is preferably a pressure-sensitive adhesive layer. The adhesive layer for bonding adjacent members together may be an adhesive layer or a pressure-sensitive adhesive layer. In one embodiment, at least one selected from the first adhesive layer, the second adhesive layer, and the third adhesive layer may be a pressure-sensitive adhesive layer, and two or three may be pressure-sensitive adhesive layers. The adhesive layer disposed directly adjacent to the support layer is preferably a pressure-sensitive adhesive layer, as this can suitably satisfy the storage modulus described below.

[0061] The storage modulus (23°C) of the adhesive layer disposed directly adjacent to the support layer is, for example, 0.01 MPa to 1 MPa, preferably 0.05 MPa to 0.5 MPa, and more preferably 0.08 MPa to 0.2 MPa. By using the surface bonded to the adhesive layer having such a storage modulus as the support layer, the effects of the present invention can be suitably achieved. The storage modulus can be measured, for example, by the following measurement method. <Method for Measuring Storage Modulus> A laminate having a thickness of approximately 1.5 mm obtained by laminating multiple pressure-sensitive adhesive layers is used as the measurement sample. Dynamic viscoelasticity measurement is performed under the following conditions using an "Advanced Rheometric Expansion System (ARES)" manufactured by Rheometric Scientific as the measurement device, and the storage modulus at 23°C is read from the measurement results. (Measurement conditions) Deformation mode: torsion Frequency: 1 Hz Pressure load: 100 g Heating rate: 5°C / min Temperature range: -50°C to 150°C Shape: parallel plate, 8.0 mm diameter

[0062] The pressure-sensitive adhesive layer can be formed using any suitable pressure-sensitive adhesive. Specific examples include acrylic pressure-sensitive adhesives, rubber pressure-sensitive adhesives, silicone pressure-sensitive adhesives, polyester pressure-sensitive adhesives, urethane pressure-sensitive adhesives, epoxy pressure-sensitive adhesives, and polyether pressure-sensitive adhesives. The pressure-sensitive adhesive contains a base resin and, depending on the purpose, may further contain various additives, such as crosslinking agents, polymerization initiators, polymerization catalysts, crosslinking catalysts, silane coupling agents, tackifiers, plasticizers, softeners, antidegradants, fillers, colorants, UV absorbers, antioxidants, surfactants, and antistatic agents, as long as they do not impair the properties of the present invention. Pressure-sensitive adhesives with desired properties can be prepared by adjusting the type, combination, and compounding ratio of monomers forming the base resin of the pressure-sensitive adhesive; the type, combination, and compounding amount of additives (e.g., crosslinking agents); reaction temperature; reaction time, etc. The base resin of the pressure-sensitive adhesive may be used alone or in combination of two or more types. Acrylic resins are preferably used as the base resin. Specifically, the pressure-sensitive adhesive layer is preferably made of an acrylic pressure-sensitive adhesive containing a (meth)acrylic polymer as a main component.

[0063] The thickness of the pressure-sensitive adhesive layer is, for example, 3 μm or more, preferably 5 μm or more, and for example, 50 μm or less, preferably 30 μm or less.

[0064] The pressure-sensitive adhesive layer can be formed by coating and drying a pressure-sensitive adhesive composition containing a base resin, additives such as a crosslinking agent, and a solvent. For example, the pressure-sensitive adhesive composition can be coated on a substrate such as a release liner and dried to form a pressure-sensitive adhesive layer, which can then be transferred to a target member. Alternatively, the pressure-sensitive adhesive composition can be directly coated on a target member and dried to form a pressure-sensitive adhesive layer. Drying is typically performed by heating.

[0065] The adhesive layer can be formed of any appropriate adhesive. For example, the adhesive irreversibly changes from a liquid to a solid state during the process of forming the adhesive layer, has fluidity when applied, and has the property of being cured by a curing treatment (e.g., irradiation with active energy rays, heating). As the adhesive, a curable adhesive is preferably used. As the curable adhesive, an ultraviolet curable adhesive is preferably used.

[0066] The ultraviolet-curable adhesive contains a curable monomer such as a compound having a (meth)acryloyl group or a compound having a vinyl group. Preferably, a compound having a (meth)acryloyl group is used. Here, the (meth)acryloyl group refers to an acryloyl group and / or a methacryloyl group.

[0067] The thickness of the adhesive layer is, for example, 0.1 μm to 5 μm, preferably 0.5 μm to 4 μm, and more preferably 1 μm to 3 μm.

[0068] <Support Layer> The position of the support layer 50 in the optical laminate is not limited to the illustrated example. The support layer 50 can be disposed directly adjacent to at least one adhesive layer arbitrarily selected from all adhesive layers of the optical laminate. For example, the support layer can be disposed directly adjacent to at least one adhesive layer selected from the surface adhesive layer, the first adhesive layer, the second adhesive layer, and the third adhesive layer (if present), preferably a pressure-sensitive adhesive layer. Since defects located near the display element tend to have a significant impact on visibility, the support layer can preferably be disposed directly adjacent to at least one selected from the surface adhesive layer, the first adhesive layer, and the third adhesive layer. The number of support layers included in the optical laminate is, for example, 1 to 3.

[0069] The indentation modulus of the support layer is, for example, 1 GPa or more, preferably 2 GPa or more, more preferably 3 GPa to 12 GPa, and even more preferably 4 GPa to 10 GPa. By disposing the adhesive layer directly adjacent to a support layer having such an indentation modulus, the generation of bubbles can be suitably suppressed. The indentation modulus is a value obtained by nanoindentation.

[0070] The hardness of the support layer is, for example, 0.05 GPa or more, preferably 0.1 GPa or more, more preferably 0.2 GPa to 2 GPa, and even more preferably 0.3 GPa to 1 GPa. The hardness is a value obtained by a nanoindentation method.

[0071] The amount of plastic deformation of the support layer is, for example, 200 nm or less, preferably 0 nm to 150 nm, more preferably 10 nm to 100 nm, and even more preferably 20 nm to 80 nm. The amount of plastic deformation is a value obtained by a nanoindentation method.

[0072] The support layer may be made of any suitable material capable of forming a layer having the above-described properties. For example, the support layer may be a cured layer of a curable material. In one embodiment, the support layer is a hard coat layer, which may be formed by applying a support layer-forming material (hard coat layer-forming material) to a member (e.g., a polarizing member, a first retardation member, a second retardation member, a protective member) onto which the adhesive layer is to be laminated, and then curing the applied layer. The support layer-forming material typically includes a curable compound as a layer-forming component. Examples of the curable compound include a thermosetting type and a photocurable type. Examples of the curable compound include a monomer, an oligomer, and a prepolymer. Preferably, a polyfunctional monomer or oligomer is used as the curable compound. Examples of the polyfunctional monomer or oligomer include a monomer or oligomer having two or more (meth)acryloyl groups, a urethane (meth)acrylate or a urethane (meth)acrylate oligomer, an epoxy-based monomer or oligomer, and a silicone-based monomer or oligomer.

[0073] In one embodiment, the support layer is provided directly adjacent to the polarizing element, preferably directly adjacent to the side of the polarizing element opposite to the side where the first retardation element is disposed. In this embodiment, the support layer can typically be formed on the surface of the protective layer of the absorptive polarizing film. When a thin absorptive polarizing film and a protective layer are bonded together via an adhesive layer, unevenness may occur on the surface of the resulting polarizing element (protective layer surface) due to shrinkage during curing. In contrast, the occurrence of such unevenness can be suppressed by bonding a support-layer-attached protective layer, on which a support layer has been formed in advance, to the absorptive polarizing film via an adhesive layer. Alternatively, when the absorptive polarizing film and the protective layer are bonded together by roll-to-roll bonding, unevenness may occur in the resulting polarizing element due to process contamination. In contrast, by forming a support layer on the surface of the protective layer of a polarizing element including an absorptive polarizing film and a protective layer bonded together via an adhesive layer, the unevenness can be filled and a flat surface can be formed. By providing a support layer directly adjacent to the polarizing member in this manner, unevenness on the surface of the polarizing member can be suppressed, and the generation of air bubbles at the lamination interface between the uneven surface and the adhesive layer (e.g., pressure-sensitive adhesive layer) can be effectively suppressed.

[0074] The thickness of the support layer is, for example, 0.5 μm to 15 μm, preferably 1 μm to 12 μm, and more preferably 3 μm to 10 μm.

[0075] <Method for Producing Optical Laminate> The optical laminate can be produced, for example, by laminating each component via an adhesive layer. In one embodiment, the optical laminate can be produced by a method including producing a support-layer-attached polarizing member having a polarizing member including an absorptive polarizing film and a protective layer disposed on at least one side of the absorptive polarizing film and a support layer disposed directly adjacent to the protective layer of the polarizing member, and laminating an adhesive layer (e.g., a pressure-sensitive adhesive layer) on the support layer side of the support-layer-attached polarizing member.

[0076] The present invention will be described in detail below using examples, but the present invention is not limited to these examples. The thickness and retardation values ​​were measured using the following measurement methods. Unless otherwise specified, "parts" and "%" are based on weight. <Thickness> Thicknesses of 10 μm or less were measured using a scanning electron microscope (manufactured by JEOL Ltd., product name "JSM-7100F"). Thicknesses exceeding 10 μm were measured using a digital micrometer (manufactured by Anritsu Corporation, product name "KC-351C"). <Retardation Value> Retardation values ​​at each wavelength at 23°C were measured using a retardation measurement device (KOBRA manufactured by Oji Scientific Instruments Co., Ltd.).

[0077] [Production Example 1: Preparation of λ / 4 Member A] Polymerization was carried out using a batch polymerization apparatus consisting of two vertical reactors equipped with stirring blades and reflux condensers controlled at 100° C. The polymerization mixture contained 29.60 parts by mass (0.046 mol) of bis[9-(2-phenoxycarbonylethyl)fluoren-9-yl]methane, 29.21 parts by mass (0.200 mol) of isosorbide (ISB), 42.28 parts by mass (0.139 mol) of spiroglycol (SPG), 63.77 parts by mass (0.298 mol) of diphenyl carbonate (DPC), and 1.19×10 calcium acetate monohydrate as a catalyst. -2 Parts by mass (6.78×10 -5mol) was charged. After purging the reactor with nitrogen under reduced pressure, heating was performed with a heat medium, and stirring was initiated when the internal temperature reached 100°C. 40 minutes after the start of the temperature increase, the internal temperature reached 220°C, and while controlling to maintain this temperature, pressure reduction was initiated. 90 minutes after reaching 220°C, the pressure was reduced to 13.3 kPa. Phenol vapor by-produced during the polymerization reaction was introduced into a reflux condenser at 100°C, and a small amount of monomer components contained in the phenol vapor were returned to the reactor, while uncondensed phenol vapor was introduced into a condenser at 45°C and recovered. Nitrogen was introduced into the first reactor, and the pressure was temporarily restored to atmospheric pressure. The oligomerized reaction liquid in the first reactor was then transferred to the second reactor. Next, heating and pressure reduction in the second reactor were initiated, and the internal temperature reached 240°C and the pressure reached 0.2 kPa in 50 minutes. Polymerization was then allowed to proceed until the predetermined stirring power was achieved. When the predetermined power was reached, nitrogen was introduced into the reactor to restore pressure, and the polyester carbonate resin produced was extruded into water, and the strands were cut to obtain pellets.

[0078] The obtained polyester carbonate resin (pellets) was vacuum dried at 80 ° C. for 5 hours, and then a film-forming device equipped with a single-screw extruder (manufactured by Toshiba Machine Co., Ltd., cylinder set temperature: 250 ° C.), a T-die (width 200 mm, set temperature: 250 ° C.), a chill roll (set temperature: 120-130 ° C.), and a winder was used to produce a long resin film having a thickness of 135 μm. The obtained long resin film was stretched in the width direction at a stretching temperature of 143 ° C. and a stretching ratio of 2.8 times to obtain a stretched film (λ / 4 member A) having a thickness of 48 μm. The Re (550) of the obtained stretched film was 143 nm, Re (450) / Re (550) was 0.86, and the Nz coefficient was 1.12.

[0079] [Production Example 2: Preparation of Protective Member A] An antireflection layer-forming material shown below was applied to an acrylic film (thickness: 40 μm) having a lactone ring structure and heated at 80° C. for 1 minute. After heating, the coating layer was irradiated with a high-pressure mercury lamp at an integrated light intensity of 300 mJ / cm 2 The coating layer was cured by irradiating it with ultraviolet light of 1000 W at ...

[0080] (Antireflection Layer-Forming Material) 100 parts by weight of a polyfunctional acrylate containing pentaerythritol triacrylate as a main component (manufactured by Osaka Organic Chemical Industry Ltd., trade name "Viscoat #300", solid content 100% by weight), 150 parts by weight of hollow nanosilica particles (manufactured by JGC Catalysts and Chemicals Industries, Ltd., trade name "Surulia 5320", solid content 20% by weight, weight average particle diameter 75 nm), 50 parts by weight of solid nanosilica particles (manufactured by Nissan Chemical Industries, Ltd., trade name "MEK-2140Z-AC", solid content 30% by weight, weight average particle diameter 10 nm), 12 parts by weight of a fluorine-containing additive (manufactured by Shin-Etsu Chemical Co., Ltd., trade name "KY-1203", solid content 20% by weight), and 3 parts by weight of a photopolymerization initiator (manufactured by BASF, trade name "OMNIRAD907", solid content 100% by weight) were mixed. To the mixture was added a mixed solvent of TBA (tertiary butyl alcohol), MIBK (methyl isobutyl ketone), and PMA (propylene glycol monomethyl ether acetate) in a weight ratio of 60:25:15 as a dilution solvent, so that the total solid content was 4 wt %, and the mixture was stirred to prepare an anti-reflection layer-forming material.

[0081] [Manufacturing Example 3: Preparation of Polarizing Member A with Support Layer] 1. Preparation of Absorptive Polarizing Film A long, amorphous, isophthalic copolymerized polyethylene terephthalate film (thickness: 100 μm) with a water absorption rate of 0.75% and a Tg of approximately 75°C was used as the thermoplastic resin substrate. One side of the resin substrate was subjected to a corona treatment. A PVA-based resin (a 9:1 mixture of polyvinyl alcohol (degree of polymerization: 4200, degree of saponification: 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., trade name "GOHSEFIRMER Z410") was prepared by mixing 100 parts by weight of the resin with 13 parts by weight of potassium iodide, and the resulting solution was dissolved in water to prepare an aqueous PVA solution (coating solution). The PVA aqueous solution was applied to the corona-treated surface of the resin substrate and dried at 60°C to form a 13 μm-thick PVA-based resin layer, producing a laminate. The resulting laminate was free-end uniaxially stretched 2.4 times in the longitudinal direction (machine direction) between rolls with different peripheral speeds in an oven at 130°C (in-air auxiliary stretching treatment). The laminate was then immersed in an insolubilizing bath (a boric acid aqueous solution obtained by blending 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40°C for 30 seconds (insolubilization treatment). The laminate was then immersed in a dyeing bath (an iodine aqueous solution obtained by blending iodine and potassium iodide in a weight ratio of 1:7 with 100 parts by weight of water) at a liquid temperature of 30°C for 60 seconds while adjusting the concentration so that the final polarizing film had a single transmittance (Ts) of 43.0% (dyeing treatment). The laminate was then immersed in a crosslinking bath (a boric acid aqueous solution obtained by blending 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40°C for 30 seconds (crosslinking treatment). The laminate was then immersed in a boric acid aqueous solution (boric acid concentration 4.0 wt%, potassium iodide concentration 5.0 wt%) at a liquid temperature of 70°C and uniaxially stretched in the longitudinal direction (longitudinal direction) between rolls with different peripheral speeds to a total stretch ratio of 5.5 (underwater stretching treatment). The laminate was then immersed in a cleaning bath (aqueous solution obtained by blending 4 parts by weight of potassium iodide with 100 parts by weight of water) at a liquid temperature of 20°C (washing treatment). Then, while drying in an oven maintained at 90°C, it was brought into contact with a SUS heated roll maintained at a surface temperature of 75°C for about 2 seconds (drying shrinkage treatment). The shrinkage rate of the laminate in the width direction due to the drying shrinkage treatment was 5.2%.In this way, an absorptive polarizing film having a thickness of 5 μm was formed on the resin substrate.

[0082] 2. Preparation of a protective layer with a support layer The following support layer-forming material was applied to an acrylic film (thickness: 40 μm) having a lactone ring structure, heated at 90° C. for 1 minute, and then irradiated the heated coating layer with a high-pressure mercury lamp at an integrated light intensity of 300 mJ / cm 2 The coating layer was cured by irradiating it with ultraviolet light of 1000 kJ / cm. This gave an acrylic film having a 7 μm thick support layer (hard coat layer) formed on one side thereof as a support layer-attached protective layer.

[0083] (Support Layer-Forming Material) A support layer-forming material was prepared by mixing 50 parts of a urethane acrylic oligomer (manufactured by Shin-Nakamura Chemical Co., Ltd., "NK Oligo UA-53H"), 30 parts of a polyfunctional acrylate mainly composed of pentaerythritol triacrylate (manufactured by Osaka Organic Chemical Industry Ltd., trade name "Viscoat #300"), 20 parts of 4-hydroxybutyl acrylate (manufactured by Osaka Organic Chemical Industry Ltd.), 1 part of a leveling agent (manufactured by DIC Corporation, "GRANDIC PC4100"), and 3 parts of a photopolymerization initiator (manufactured by Ciba Japan KK, "Irgacure 907") and diluting with methyl isobutyl ketone to a solids concentration of 50%.

[0084] 3. Preparation of Polarizing Member: The above-mentioned support layer-attached protective layer was attached to the surface of the absorptive polarizing film of the laminate of [resin substrate / absorptive polarizing film] obtained in 1 above, via a UV-curable adhesive, with the acrylic film facing the absorptive polarizing film. Specifically, the curable adhesive was applied to a thickness of 1.0 μm, and the layers were attached using a rolling mill. The adhesive was then cured by irradiating the support layer-attached protective layer side with UV light. Next, the resin substrate was peeled from the absorptive polarizing film, and an acrylic film (thickness: 40 μm) having a lactone ring structure was attached to the peeled surface in the same manner as above. In this way, a support layer-attached polarizing member A having a configuration of [support layer / acrylic film / absorptive polarizing film / acrylic film] was obtained. In the support layer-attached polarizing member A, the support layer was provided directly adjacent to the polarizing member (more specifically, directly adjacent to the surface of the protective layer).

[0085] [Production Example 4A: Preparation of Pressure-Sensitive Adhesive Layer A] A four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser was charged with a monomer mixture containing 91.5 parts of butyl acrylate, 3 parts of acrylic acid, 0.5 parts of 4-hydroxybutyl acrylate, and 5 parts of acryloylmorpholine. Furthermore, 100 parts of this monomer mixture was charged with 0.1 parts of 2,2'-azobisisobutyronitrile as a polymerization initiator along with 100 parts of ethyl acetate. Nitrogen gas was introduced into the flask with gentle stirring to replace the atmosphere with nitrogen, and the liquid temperature in the flask was maintained at around 55°C, allowing the polymerization reaction to proceed for 8 hours. Ethyl acetate was then added to the resulting reaction solution to adjust the solids concentration to 12 wt%, thereby preparing a solution of an acrylic polymer having a weight-average molecular weight (Mw) of 2,500,000. A pressure-sensitive adhesive composition was prepared by blending 0.3 parts of a peroxide-based crosslinking agent, benzoyl peroxide (trade name: Niper BMT, manufactured by NOF Corporation), 0.2 parts of a trimethylolpropane / tolylene diisocyanate adduct (trade name: Coronate L, manufactured by Tosoh Corporation), and 0.2 parts of a silane coupling agent (trade name: KBM403, manufactured by Shin-Etsu Chemical Co., Ltd.), per 100 parts of the solids content of the obtained acrylic polymer solution. The obtained pressure-sensitive adhesive composition was applied to the release surface of a release liner, which was a PET film whose release surface had been treated with a release agent, and dried to form a pressure-sensitive adhesive layer A having a thickness of 5 μm.

[0086] [Production Example 4B: Preparation of Pressure-Sensitive Adhesive Layer B] A monomer mixture containing 94.9 parts by weight of butyl acrylate, 5 parts by weight of acrylic acid, and 0.1 parts by weight of 2-hydroxyethyl acrylate was charged into a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser. Furthermore, 0.3 parts by weight of dibenzoyl peroxide as a polymerization initiator was charged together with ethyl acetate for 100 parts of this monomer mixture. Nitrogen gas was introduced into the flask with gentle stirring to replace the atmosphere with nitrogen, and the liquid temperature in the flask was maintained at around 60°C, allowing the polymerization reaction to proceed for 7 hours. Ethyl acetate was then added to the resulting reaction solution to adjust the solids concentration to 30% by weight, thereby preparing an acrylic polymer solution having a weight-average molecular weight (Mw) of 2,200,000. A pressure-sensitive adhesive composition was prepared by blending 0.2 parts of a peroxide-based crosslinking agent, benzoyl peroxide (trade name: Niper BMT, manufactured by NOF Corporation), 0.6 parts of a trimethylolpropane / tolylene diisocyanate adduct (trade name: Coronate L, manufactured by Tosoh Corporation), and 0.2 parts of a silane coupling agent (trade name: KBM403, manufactured by Shin-Etsu Chemical Co., Ltd.), per 100 parts of the solids content of the obtained acrylic polymer solution. The obtained pressure-sensitive adhesive composition was applied to the release surface of a release liner, which was a PET film whose release surface had been treated with a release agent, and dried to form a pressure-sensitive adhesive layer B having a thickness of 15 μm.

[0087] [Example 1] Pressure-sensitive adhesive layers B were bonded together with release liners to both sides of a λ / 4 member A serving as a second retardation member. The release liner on one side was peeled off, and the exposed pressure-sensitive adhesive layer B was bonded to the support layer side surface of the support layer-attached polarizing member A, thereby obtaining a laminate 1 having a layered structure of [release liner / pressure-sensitive adhesive layer B / second retardation member / pressure-sensitive adhesive layer B / support layer / polarizing member]. At this time, the layers were bonded such that the absorption axis of the absorptive polarizing film and the slow axis of the λ / 4 member A formed an angle of 45°.

[0088] The protective member A was bonded to one side of the λ / 4 member A as a first retardation member via the pressure-sensitive adhesive layer B. The acrylic film of the protective member A was bonded to the λ / 4 member A side. This resulted in a laminate 2 having a laminated structure of [first retardation member / pressure-sensitive adhesive layer B / protective member A].

[0089] Laminate 2 was bonded to the polarizing member side of laminate 1 via pressure-sensitive adhesive layer A. At this time, the laminates were bonded so that the first retardation member of laminate 2 was located on the pressure-sensitive adhesive layer A side and so that the angle between the slow axis of λ / 4 member A of laminate 1 and the slow axis of λ / 4 member A of laminate 2 was 0°. This resulted in an optical laminate A having a layered structure of [release liner / pressure-sensitive adhesive layer B / second retardation member / pressure-sensitive adhesive layer B / support layer / polarizing member / pressure-sensitive adhesive layer A / first retardation member / pressure-sensitive adhesive layer B / protective member A]. In optical laminate A, a support layer was provided directly adjacent to the protective layer of the absorptive polarizing film, and pressure-sensitive adhesive layer B was disposed directly adjacent to the support layer.

[0090] <Evaluation of bubbles> When the obtained optical laminate A was observed under a microscope, it was found that bubbles of 10 μm or more were generated at the interface between the support layer and the pressure-sensitive adhesive layer B at 1 bubble per 100 cm. 2 This was within the practically acceptable range.

[0091] <Evaluation of Support Layer Characteristics> Polarizing member A with a support layer was cut into a 10 mm x 10 mm square to prepare a measurement sample. Using this measurement sample, nanoindentation measurement was performed on the support layer under the following conditions: Measurement device: Hysitron Inc., product name "Triboindenter" Indenter used: Berkovich (triangular pyramid type) Measurement method: Single indentation measurement Measurement temperature: Room temperature (approximately 25°C) Indentation depth setting: 200 nm Indentation speed: 20 nm / s

[0092] From the measurement results, the indentation modulus (S√π / 2√A), hardness (Pmax / A), and plastic deformation were calculated using the software (triboscan) attached to the measuring device (S: contact stiffness, A: contact projected area, Pmax: maximum load). The average values ​​of N = 3 were used as the indentation modulus, hardness, and plastic deformation of the support layer. As a result, the indentation modulus of the support layer was 6.01 GPa, the hardness was 0.383 GPa, and the plastic deformation was 47.0 nm.

[0093] The present invention is not limited to the above-described embodiment, and various modifications are possible. For example, the configurations shown in the above-described embodiment can be replaced with configurations that are substantially the same as those shown in the above-described embodiment, that have the same effects, or that can achieve the same purpose.

[0094] The optical laminate according to the embodiment of the present invention can be suitably used in a display system such as VR goggles, for example.

[0095] 2 Display system, 4 Lens portion, 12 Display element, 14 Reflective polarizing member, 16 First lens portion, 18 Half mirror, 20 First phase difference member, 22 Lens portion phase difference member, 24 Second lens portion, 30 Protective member, 42 Surface adhesive layer, 44 First adhesive layer, 46 Second adhesive layer, 48 Third adhesive layer, 50 Support layer, 60 Second phase difference member, 100 Optical laminate

Claims

1. An optical laminate comprising a polarizing member having an absorptive polarizing film and a protective layer disposed on at least one side of the polarizing film, and a first phase difference member, wherein the optical laminate further comprises a support layer having an indentation elastic modulus of 1 GPa or more, and an adhesive layer is disposed directly adjacent to the support layer.

2. The optical laminate according to claim 1, comprising, in this order, a surface adhesive layer, the polarizing member, a first adhesive layer, the first phase difference member, a second adhesive layer, and a protective member.

3. The optical laminate of claim 2, wherein at least one selected from the surface adhesive layer, the first adhesive layer, and the second adhesive layer is disposed directly adjacent to the support layer.

4. The optical laminate described in claim 1, comprising, in this order, a surface adhesive layer, a second phase difference member, a third adhesive layer, the polarizing member, a first adhesive layer, the first phase difference member, a second adhesive layer, and a protective member.

5. The optical laminate of claim 4, wherein at least one selected from the surface adhesive layer, the first adhesive layer, the second adhesive layer, and the third adhesive layer is disposed directly adjacent to the support layer.

6. The optical laminate according to claim 1, wherein the support layer is a hard coat layer.

7. The optical laminate according to claim 1, wherein the support layer has a thickness of 0.5 μm to 15 μm.

8. The optical laminate according to claim 1, wherein the support layer is provided directly adjacent to the polarizing member on the side opposite to the side on which the first phase difference member is disposed.

9. The optical laminate according to claim 1, wherein the adhesive layer disposed directly adjacent to the support layer has an elastic modulus of 0.01 MPa to 1 MPa.

10. A display system comprising an optical laminate according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Production and use of clear heat-resistant resin

    JP2000230016A

  • Method of manufacturing for transparent heat resistant resin and use of the same

    JP2001151814A

  • Transparent thermoplastic resin laminate

    JP2002120326A

  • Thermoplastic resin laminate

    JP2002254544A

  • Homeotropic alignment liquid-crystalline composition, method for producing homeotropic alignment liquid crystal film and homeotropic alignment liquid crystal film

    JP2002333642A