Fluorescent powder and light-emitting device
By optimizing the particle size distribution and composition of europium-activated β-type sialon phosphor powder, the challenges of enhancing luminous flux and reducing chromaticity variations in light-emitting devices are addressed, resulting in improved light quality with reduced phosphor powder usage.
Patent Information
- Application Number
- PCT/JP2024/009868
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-13
- Publication Date
- 2024-10-03
AI Technical Summary
Existing light-emitting devices using europium-activated β-type sialon phosphor struggle to simultaneously enhance total luminous flux and reduce chromaticity variations.
A phosphor powder with specific particle size distribution characteristics, where the 10% cumulative diameter (D10), 50% cumulative diameter (D50), and 90% cumulative diameter (D90) are optimized within certain ranges, and the span value (D90-D10)/D50 is controlled to be less than 1.10, along with a composition represented by the general formula Si12−a Al a O b N16−b:Eu x, where a, b, and x are adjusted within specific limits, to improve luminous flux and chromaticity stability.
The optimized phosphor powder enhances the total luminous flux and reduces chromaticity variations in light-emitting devices by adjusting the particle size distribution and composition, resulting in improved light quality with reduced phosphor powder usage.
Smart Images

Figure JP2024009868_03102024_PF_FP_ABST
Abstract
Description
Phosphor powder and light-emitting device
[0001] The present disclosure relates to phosphor powders and light emitting devices.
[0002] Europium-activated β-sialon phosphors (also referred to as "europium-activated β-sialon phosphors") are known as phosphors used in light-emitting devices such as LED packages. Studies are being conducted to improve the performance of light-emitting devices by controlling the particle shape, etc., of the phosphors used in the light-emitting devices.
[0003] For example, Patent Document 1 discloses a compound having the general formula: Eu a Si b Al c O d N e (wherein a is a number satisfying 0.005≦a≦0.4, b+c=12, d+e=16), and 60% or more of the phosphor particle group is composed of phosphor particles (1) having a value obtained by dividing the major axis by the minor axis of more than 1.0 and not more than 3.0. It is also disclosed that the phosphor particle group may have a median diameter in the range of 6 to 20 μm.
[0004] International Publication No. 2009 / 008250
[0005] Light emitting devices are required to have sufficient brightness (total luminous flux) while also having small variations in chromaticity. However, according to the studies of the present inventors, it is difficult to achieve both an improvement in total luminous flux and a reduction in variations in chromaticity in light emitting devices that use phosphor powder containing a europium-activated β-sialon phosphor.
[0006] Therefore, an object of the present disclosure is to provide a phosphor powder that can improve the total luminous flux of a light-emitting device and reduce variations in chromaticity.
[0007] As a result of intensive research, the inventors have found that by adjusting the 50% cumulative diameter in the volume-based cumulative particle size distribution of the phosphor powder and the span value ((D90-D10) / D50), which indicates the relationship between the 10% cumulative diameter, the 50% cumulative diameter, and the 90% cumulative diameter, within each specific numerical range, the total luminous flux of the light-emitting device can be improved and the variation in chromaticity can be reduced.
[0008] The present disclosure provides the following [1] to [3]. [1] A phosphor powder containing particles of a europium-activated β-sialon phosphor, wherein, when the 10% cumulative diameter, the 50% cumulative diameter, and the 90% cumulative diameter in a volume-based cumulative particle size distribution are D10, D50, and D90, respectively, D50 is more than 20.0 μm and not more than 30.0 μm, and (D90-D10) / D50 is less than 1.10. [2] The phosphor powder according to [1], wherein the europium-activated β-sialon phosphor has a composition represented by the following general formula (1): Si 12-a Al a O b N 16-b :Eu x ... (1) [In general formula (1), a, b, and x represent numerical values satisfying 0<a≦3, 0<b≦3, and 0<x≦0.1, respectively.] [3] A light emitting device comprising a light emitting element that emits primary light, and a wavelength converter that absorbs a part of the primary light and emits secondary light having a wavelength longer than that of the primary light, wherein the wavelength converter contains the phosphor powder according to [1] or [2].
[0009] According to the present disclosure, it is possible to provide a phosphor powder that can improve the total luminous flux of a light emitting device and reduce variations in chromaticity.
[0010] FIG. 1 is a schematic cross-sectional view showing an example of a light emitting device.
[0011] Hereinafter, embodiments of the present disclosure will be described. However, the following embodiments are merely examples for explaining the present disclosure, and are not intended to limit the present disclosure to the following contents.
[0012] Unless otherwise specified, the materials exemplified in this specification can be used alone or in combination of two or more.
[0013] One embodiment of the phosphor powder is a phosphor powder containing particles of a europium-activated β-sialon phosphor, in which, when the 10% cumulative diameter, the 50% cumulative diameter, and the 90% cumulative diameter in a volume-based cumulative particle size distribution are defined as D10, D50, and D90, respectively, D50 is greater than 20.0 μm and not more than 30.0 μm, and (D90−D10) / D50 is less than 1.10.
[0014] The particles of the europium-activated β-sialon phosphor are particulate europium-activated β-sialon phosphors. The particles of the europium-activated β-sialon phosphor may contain, as a main crystal, a crystal having the same crystal structure as β-sialon, or may be composed of crystals having the same crystal structure as β-sialon. The particles of the europium-activated β-sialon phosphor may contain a different phase within a range that does not detract from the spirit of the present disclosure.
[0015] The europium-activated β-sialon phosphor may have a composition represented by the following general formula (1): Si 12-a Al a O b N 16-b :Eu x ... (1) [In general formula (1), a, b, and x respectively represent values satisfying 0<a≦3, 0<b≦3, and 0<x≦0.1.]
[0016] In the general formula (1), a may be 0.005 or more, 0.01 or more, 0.1 or more, or 0.2 or more, and may be 1.0 or less, 0.8 or less, 0.6 or less, 0.5 or less, or 0.4 or less. Furthermore, b may be 0.005 or more, 0.01 or more, 0.1 or more, or 0.2 or more, and may be 1.0 or less, 0.8 or less, 0.6 or less, 0.5 or less, or 0.4 or less. a and b may be different from each other or may be the same. x may be 0.005 or more, or 0.01 or more, and may be 0.08 or less, 0.06 or less, or 0.05 or less. a, b, and x in the general formula (1) can be adjusted by adjusting the composition and composition ratio of the raw materials.
[0017] In the composition of the europium-activated β-sialon phosphor, the contents of nitrogen atoms (N) and oxygen atoms (O) can be quantified using an oxygen / nitrogen analyzer, and the contents of europium (Eu), silicon (Si), and aluminum (Al) can be confirmed by quantitative elemental analysis using an ICP optical emission spectrometer.
[0018] The 10% cumulative diameter (D10) in the volume-based cumulative particle size distribution of the phosphor powder may be 5.0 μm or more, 8.0 μm or more, 10.0 μm or more, 12.0 μm or more, 14.0 μm or more, 15.0 μm or more, or 16.0 μm or more from the viewpoint of further improving the total luminous flux of the light emitting device and suppressing light scattering at the particle surfaces of the phosphor powder, and may be 20.0 μm or less, 19.0 μm or less, 18.0 μm or less, or 17.0 μm or less from the viewpoint of reducing the amount (mass) of phosphor powder used in the light emitting device. When D10 is equal to or less than the upper limit, the specific surface area of the phosphor powder can be made larger, and when the phosphor powder is used in a light emitting device, it becomes possible to obtain light of the desired color with a smaller amount.
[0019] The 50% cumulative diameter (D50) in the volume-based cumulative particle size distribution of the phosphor powder is greater than 20.0 μm and less than 30.0 μm. From the viewpoints of further improving the total luminous flux of the light-emitting device and suppressing light scattering at the particle surfaces of the phosphor powder, the D50 of the phosphor powder may be 21.0 μm or more, 22.0 μm or more, 23.0 μm or more, 24.0 μm or more, 25.0 μm or more, 25.5 μm or more, or 25.8 μm or more. Furthermore, from the viewpoint of reducing the amount (mass) of phosphor powder used in the light-emitting device, the D50 of the phosphor powder may be 29.0 μm or less, 28.5 μm or less, 28.0 μm or less, 27.5 μm or less, 27.0 μm or less, or 26.5 μm or less. When the D50 is equal to or less than the upper limit, the specific surface area of the phosphor powder can be increased, and when the phosphor powder is used in a light emitting device, light of the desired color can be obtained with a smaller amount. The D50 of the phosphor powder can be adjusted within the above range, and may be, for example, 25.0 to 30.0 μm or 25.5 to 30.0 μm.
[0020] The 90% cumulative diameter (D90) in the volume-based cumulative particle size distribution of the phosphor powder may be 23.0 μm or more, 25.0 μm or more, 28.0 μm or more, 30.0 μm or more, 32.0 μm or more, 35.0 μm or more, 38.0 μm or more, 40.0 μm or more, or 41.0 μm or more, from the viewpoint of further improving the total luminous flux of the light emitting device and suppressing light scattering at the particle surfaces of the phosphor powder, and may be 50.0 μm or less, 48.0 μm or less, 46.0 μm or less, or 44.0 μm or less, from the viewpoint of reducing the amount (mass) of phosphor powder used in the light emitting device. When D90 is equal to or less than the upper limit, the specific surface area of the phosphor powder can be increased, and when the phosphor powder is used in a light emitting device, it becomes possible to obtain light of the desired color with a smaller amount.
[0021] In this specification, the 10% cumulative diameter (D10), 50% cumulative diameter (D50), and 90% cumulative diameter (D90) in the volume-based cumulative particle size distribution of the phosphor powder refer to the particle diameters at which the cumulative values from the smallest particle size in the volume-based particle size distribution curve measured by laser diffraction / scattering reach 10%, 50%, and 90%, respectively, of the total. Specifically, D10, D50, and D90 can be determined by the procedures described in the Examples section of this specification. D50, also known as the median diameter, refers to the average particle size of the target particles. D10, D50, and D90 can be controlled, for example, by adjusting the heating temperature, heating time, and other conditions during the production of the phosphor powder.
[0022] The (D90-D10) / D50 (span value) of the phosphor powder is less than 1.10. The span value of the phosphor powder may be 1.05 or less, 1.00 or less, 0.99 or less, or 0.98 or less. By setting the span value to the upper limit or less, it is possible to further reduce the variation in chromaticity of the light emitting device. Furthermore, the span value of the phosphor powder may be, for example, 0.10 or more, or 0.50 or more.
[0023] The phosphor powder has a relatively large average particle size while suppressing the span value to a range of less than 1.1. From the viewpoint of achieving a higher level of both improvement in total luminous flux and suppression of chromaticity variation in the light emitting device when manufactured, the phosphor powder may have, for example, a D50 of 25 to 30 μm and a span value of 0.10 to 1.05, a D50 of 25 to 30 μm and a span value of 0.60 to 1.05, or a D50 of 25 to 30 μm and a span value of 0.90 to 1.05.
[0024] The phosphor powder is excited by excitation light (light having a shorter wavelength than the light emitted by the phosphor powder) or the like to emit fluorescence. The emission peak wavelength of the phosphor powder may be, for example, 540 nm or more and 550 nm or less.
[0025] The chromaticity X of the phosphor powder may be, for example, 0.350 or more, 0.360 or more, or 0.370 or more, and may be 0.400 or less, 0.390 or less, or 0.380 or less. The chromaticity X of the phosphor powder can be adjusted within the above-mentioned range, and may be, for example, 0.350 to 0.400, or 0.360 to 0.390.
[0026] The chromaticity Y of the phosphor powder may be, for example, 0.580 or more, 0.590 or more, or 0.600 or more, and may be 0.630 or less, 0.620 or less, 0.615 or less, or 0.610 or less. The chromaticity Y of the phosphor powder can be adjusted within the above-mentioned range, and may be, for example, 0.580 to 0.630, or 0.590 to 0.620.
[0027] The chromaticity X and chromaticity Y of the phosphor powder refer to values calculated as the CIE chromaticity coordinate x value (chromaticity X) and y value (chromaticity Y) in the XYZ color system defined in JIS Z8781-3:2016 in accordance with JIS Z8724:2015 from data of the fluorescence spectrum of the phosphor powder in the wavelength range of 465 to 780 nm.
[0028] One example of a method for producing a phosphor powder containing particles of a europium-activated β-sialon phosphor includes a firing step of obtaining a fired product from a raw material composition containing a silicon source, an aluminum source, a europium source, and a nucleating agent, wherein at least one of the silicon source, the aluminum source, and the europium source is present as a nitride, by one or more heat treatments, and a crushing step of crushing the fired product to obtain a powder. In the crushing step, the powder obtained has a D50 of more than 20.0 μm and not more than 30.0 μm, and (D90-D10) / D50 is less than 1.10.
[0029] The raw material composition contains compounds having elements that are constituent elements of the europium-activated β-sialon, and contains at least a silicon source, an aluminum source, and a europium source. In the raw material composition, at least one of the silicon source, the aluminum source, and the europium source is a nitride. The nitride contains nitrogen, which is a constituent element of the europium-activated β-sialon, and is therefore also a nitrogen source. The silicon source refers to a compound or element containing silicon as a constituent element. The aluminum source refers to a compound or element containing aluminum as a constituent element. The europium source refers to a compound or element containing europium as a constituent element. In this specification, a compound containing silicon as a constituent element is also referred to as a silicon compound, a compound containing aluminum as a constituent element is also referred to as an aluminum compound, and a compound containing europium as a constituent element is also referred to as a europium compound. The silicon compound, the aluminum compound, and the europium compound may each be any of a nitride, an oxide, an oxynitride, a hydroxide, and a halide.
[0030] Examples of silicon compounds include silicon nitride (Si 3 N 4 ), and silicon dioxide (SiO 2) are included. When silicon nitride powder is used as the silicon compound, it is preferable to use silicon nitride powder with a high α fraction. The α fraction of the silicon nitride powder may be, for example, 80 mass% or more, 90 mass% or more, or 95 mass% or more. When the α fraction of the silicon nitride powder is within the above range, primary particle growth can be promoted. It is preferable to use silicon nitride powder with a low oxygen content. The oxygen content of the silicon nitride powder may be, for example, 3 mass% or less, 2 mass% or less, 1.5 mass% or less, or 1.3 mass% or less, based on the total mass of the silicon nitride powder. When the oxygen content of the silicon nitride powder is within the above range, the occurrence of defects in the β-sialon crystal and the main crystalline phase of the europium-activated β-sialon phosphor can be suppressed.
[0031] Examples of aluminum compounds include aluminum nitride (AlN), aluminum oxide (Al 2 O 3 ), and aluminum hydroxide (Al(OH) 3 When aluminum nitride powder is used as the aluminum compound, it is preferable to use aluminum nitride powder with a low oxygen content. The oxygen content of the aluminum nitride powder may be, for example, 3 mass % or less, 2 mass % or less, 1.5 mass % or less, or 1.0 mass % or less, based on the total mass of the aluminum nitride powder.
[0032] Examples of europium compounds include europium oxide (europium oxide), europium nitride (europium nitride), and europium halides. Examples of europium halides include europium fluoride, europium chloride, europium bromide, and europium iodide. The europium compound preferably contains europium oxide. The valence of europium in the europium compound may be divalent or trivalent.
[0033] The nucleating agent may include, for example, β-sialon, europium-activated β-sialon, etc. Adding a nucleating agent and adjusting the amount of nucleating agent can promote particle growth of the europium-activated β-sialon phosphor. Then, by increasing the particle size of the fired product and then performing a pulverization process in the pulverization step described below, the particle size can be adjusted to a predetermined span value while maintaining a predetermined average particle size. The europium-activated β-sialon serving as the nucleating agent may be prepared separately and, for example, can be obtained by the preparation method including the sintering step described above. The particle size (D50) of the nucleating agent may be, for example, 10 μm or more, or 15 μm or more, and may be less than 45 μm. The particle size of the nucleating agent can be determined in the same manner as the D50 of the phosphor powder.
[0034] The raw material composition can be prepared by weighing and mixing each compound. A dry mixing method or a wet mixing method may be used for mixing. The dry mixing method may be, for example, a method in which each component is mixed using a V-type mixer or the like. The wet mixing method may be, for example, a method in which a solvent or dispersion medium such as water is added to prepare a solution or slurry, the components are mixed, and then the solvent or dispersion medium is removed.
[0035] The heating temperature in the firing step may be, for example, 1800 to 2500°C, 1800 to 2400°C, 1850 to 2100°C, 1900 to 2100°C, 1900 to 2050°C, or 1920 to 2050°C. By setting the heating temperature in the firing step to 1800°C or higher, grain growth of the main crystalline phase of the β-sialon and europium-activated β-sialon phosphor can be promoted, and the amount of europium dissolved in the solid solution can be made more sufficient. By setting the heating temperature in the firing step to 2500°C or lower, decomposition of the β-sialon crystal and the main crystalline phase of the europium-activated β-sialon phosphor can be sufficiently suppressed.
[0036] The heating time in the firing step is preferably longer from the viewpoint of promoting the growth of primary particles of the main crystalline phase of the β-sialon and europium-activated β-sialon phosphor. However, if the heating time is too long, the production efficiency decreases. Therefore, the heating time may be, for example, 1 to 30 hours, 3 to 25 hours, or 5 to 20 hours.
[0037] The raw material composition may be heated in a nitrogen atmosphere in the firing step, for example. Heating under conditions of high nitrogen partial pressure can suppress decomposition of silicon nitride at high temperatures. Furthermore, treating at high temperatures can promote particle growth. The raw material composition may be heated under pressure in the firing step, for example. The pressure (absolute pressure) in this case may be, for example, 0.01 to 200 MPa, 0.02 to 200 MPa, 0.05 to 200 MPa, 0.1 to 100 MPa, 0.5 to 100 MPa, 0.5 to 50 MPa, 0.5 to 10 MPa, or 0.5 to 1 MPa.
[0038] The fired product obtained by the firing step may have β-sialon crystals, and may contain a solid solution in which an element serving as a luminescence center is dissolved in a part of the crystals, and may itself be capable of emitting fluorescence. That is, the fired product may contain a europium-activated β-sialon phosphor.
[0039] For example, a jet mill can be used for the pulverization in the pulverization step. The pulverization of the fired product is carried out in two or more stages. By dividing the pulverization process into two or more stages in this way, it becomes easier to adjust the particle size, for example by preventing excessive pulverization. The number of pulverization steps may be two or more, but may also be three or more. The number of pulverization steps may be, for example, five or less. In this specification, "pulverization" also includes "disintegration."
[0040] Each pulverization may be performed under conditions where the air pressure is 0.2 MPa or more, or 0.4 MPa or more. Each pulverization may be performed under conditions where the air pressure is 0.8 MPa or less, or 0.6 MPa or less. Each pulverization may be performed under conditions where the air pressure is, for example, 0.2 to 0.8 MPa. Furthermore, each pulverization may be performed under conditions where the supply rate of the calcined product is 1.0 kg / h or more, 2.0 kg / h or more, or 2.5 kg / h or more. Each pulverization may be performed under conditions where the supply rate of the calcined product is 10.0 kg / h or less, 5.0 kg / h or less, or 3.5 kg / h or less. Each pulverization may be performed under conditions where the supply rate of the calcined product is 1.0 to 10.0 kg / h. Multiple pulverizations may be performed under the same conditions, or under different conditions.
[0041] In addition to the firing step and the pulverization step, the manufacturing method may further include an annealing step in which the fired product is heated at a temperature lower than the heating temperature in the firing step to obtain an annealed product. The fired product heated in the annealing step may be the fired product after the pulverization step (in other words, the pulverized fired product). When the manufacturing method includes the annealing step, the luminous efficiency of the manufactured phosphor powder can be further improved. In addition, the rearrangement of elements can eliminate strain and defects in the β-sialon, thereby improving transparency. Note that during the annealing step, heterogeneous phases may be generated, but these can be removed by treatment with an acid, as described below.
[0042] The annealing step can be carried out in an atmosphere selected from the group consisting of an inert gas, a reducing gas, a mixed gas thereof, and a non-oxidizing atmosphere. Examples of inert gases include rare gases (such as argon gas) and nitrogen gas. Examples of reducing gases include hydrogen gas, carbon monoxide gas, hydrocarbon gas, and ammonia gas. Examples of mixed gases include mixed gases of the above inert gases and the above reducing gases. The non-oxidizing atmosphere is preferably a non-oxidizing atmosphere other than pure nitrogen, such as a vacuum. The annealing step is preferably carried out in a hydrogen gas atmosphere or an argon atmosphere.
[0043] The annealing step may be performed under atmospheric pressure or under pressure. The heat treatment temperature in the annealing step is not particularly limited, but is preferably 1100 to 1700°C, more preferably 1100 to 1650°C, and even more preferably 1200 to 1600°C.
[0044] The heating time in the annealing step may be, for example, 1 to 20 hours, 3 to 15 hours, or 5 to 10 hours.
[0045] In the annealing step, other components may be added to the fired product before heating it. That is, the fired product may be heated as a mixture of the fired product and other components. Examples of the other components include compounds containing elements constituting the europium-activated β-sialon phosphor (at least one element selected from the group consisting of silicon, aluminum, europium, oxygen, and nitrogen).
[0046] Examples of compounds containing the elements that make up the europium-activated β-sialon phosphor as constituent elements include the above-mentioned silicon compounds (silicon dioxide, etc.), aluminum compounds (aluminum oxide, etc.), and europium compounds (europium oxide, europium fluoride, etc.).
[0047] The above-mentioned manufacturing method may further include a step of treating the annealed product with at least one of an acid and an alkali, a classification step of adjusting the particle size of the fired product or the annealed product (including the annealed product after being treated with at least one of an acid and an alkali), etc.
[0048] The process of treating the annealed product with acid is called the acid treatment process, and the process of treating the annealed product with alkali is called the alkali treatment process. The acid treatment process or alkali treatment process can, for example, reduce the crystal defect density in the phosphor contained in the annealed product, remove silicon present on the surface of the solid solution formed by thermal decomposition of β-sialon, and remove AlN polytypoid, a pseudo-polymorph of aluminum nitride (AlN) produced as a by-product during the preparation of the fired product. Furthermore, if other components are added in the annealing process, heterogeneous phases other than the europium-activated β-sialon phosphor derived from the added components can be removed. The acid may include, for example, hydrofluoric acid, nitric acid, hydrochloric acid, etc. The acid may be a mixed acid of hydrofluoric acid and nitric acid. The alkali may include, for example, sodium hydroxide, etc.
[0049] The classification step may be carried out by, for example, either a wet classification method or a dry classification method. Examples of wet classification include an elutriation classification method in which the fired product or annealed product is added to a solvent such as a mixed solvent containing ion-exchanged water and a dispersant (e.g., sodium hexametaphosphate) or a mixed solvent containing ion-exchanged water and aqueous ammonia, and the mixture is stirred and then allowed to stand, and fine powder having a small particle size is separated together with the supernatant liquid.
[0050] The phosphor powder of the present disclosure, which contains particles of a europium-activated β-sialon phosphor, can be used alone or in combination with other phosphor powders. The phosphor powder of the present disclosure, which contains particles of a europium-activated β-sialon phosphor, has excellent excitation light absorption rate when dispersed in a cured resin, and can therefore be used in light-emitting devices such as LED packages.
[0051] One embodiment of the light emitting device is a light emitting device including a light emitting element that emits primary light and a wavelength converter that absorbs a portion of the primary light and emits secondary light having a wavelength longer than the wavelength of the primary light. The wavelength converter includes the phosphor powder described above. The light emitting element and the wavelength converter may be sealed with a sealing resin or the like.
[0052] Fig. 1 is a schematic cross-sectional view showing an example of a light-emitting device. The light-emitting device shown in Fig. 1 is an example of an optical semiconductor device classified as a surface-mount type. The light-emitting device 100 includes a substrate 10, a light-emitting element 40 electrically connected to a metal layer 20 of the substrate 10, a reflector 30 provided on the surface of the substrate 10 so as to surround the light-emitting element 40, and a transparent sealing resin 60 filled in a recess formed by the substrate 10 and the reflector 30 to seal the light-emitting element 40. Phosphor powder 52 containing particles of the above-mentioned europium-activated β-sialon phosphor and other phosphor powders 54 are dispersed in the transparent sealing resin 60.
[0053] The substrate 10 has a metal layer 20 on a portion of its surface, and the metal layer 20 serves as an electrode that is electrically connected to a light-emitting element 40 arranged on the surface of the substrate 10. The light-emitting element 40 is die-bonded to the metal layer 20 on either the anode side or the cathode side, and is electrically connected to the metal layer 20 via a die-bonding material 42. The light-emitting element 40 is electrically connected to the metal layer 20 on either the anode side or the cathode side via a bonding wire 44.
[0054] The reflective portion 30 is filled with a transparent sealing resin 60 for sealing the light-emitting element 40, and reflects the light (excitation light) emitted from the light-emitting element 40, as well as the fluorescence emitted from the phosphor powder 52 and other phosphor powders 54 in response to the light, toward the surface side of the light-emitting device 100.
[0055] The light-emitting element 40 may emit light (primary light, excitation light) that can excite at least one of the phosphor powder 52 and the other phosphor powder 54. The light-emitting element 40 may be, for example, a near-ultraviolet light-emitting diode (near-ultraviolet LED), an ultraviolet light-emitting diode (ultraviolet LED), or a blue light-emitting diode (blue LED). A plurality of light-emitting elements 40 may be provided.
[0056] The light emitting device 100 includes, in addition to the phosphor powder 52, another phosphor powder 54. The other phosphor powder 54 may include, for example, a phosphor other than the europium-activated β-sialon phosphor described above (such as a red phosphor, a yellow phosphor, a green phosphor, or a blue phosphor). In another example, the light emitting device 100 may include only the phosphor powder 52 containing particles of the europium-activated β-sialon phosphor as the phosphor powder.
[0057] Examples of the transparent sealing resin 60 include silicone resin, epoxy resin, polyvinyl resin, polyethylene, polypropylene, and polyester.
[0058] In the above example, the light emitting device has been described as an optical semiconductor device classified as a surface mount type, but the light emitting device is not limited to this. The light emitting device may be, for example, a light source for analysis, a signal device, or a light source for backlighting a liquid crystal display or liquid crystal panel.
[0059] Although several embodiments have been described above, the present disclosure is not limited to the above embodiments. Furthermore, the descriptions of the above embodiments can be applied to each other.
[0060] The present disclosure will be described in more detail below with reference to examples and comparative examples, although the present disclosure is not limited to the following examples.
[0061] In the following examples and comparative examples, the following raw materials were used: α-type silicon nitride powder (manufactured by UBE Inc., trade name "UBE Silicon Nitride SN-E10", oxygen content based on the total mass of the silicon nitride powder: 1.0 mass%), aluminum nitride powder (manufactured by Tokuyama Corporation, trade name "Aluminum Nitride Powder E Grade", oxygen content based on the total mass of the aluminum nitride powder: 0.8 mass%), aluminum oxide powder (manufactured by Taimei Chemical Industry Co., Ltd., trade name "Low Temperature Sinterable Alumina TM-DAR"), and europium (III) oxide powder (manufactured by Shin-Etsu Chemical Co., Ltd., trade name "Europium Oxide Fine Powder RU Type").
[0062] [Preparation of Nucleating Agent] Using a micro V-type mixer (S-3 model, manufactured by Tsutsui Scientific Instruments Co., Ltd.), 95.20 mass% of α-type silicon nitride powder, 2.88 mass% of aluminum nitride powder, 0.92 mass% of aluminum oxide powder, and 1.00 mass% of europium oxide powder were mixed. The resulting mixture was passed through a sieve with a mesh size of 250 μm to remove agglomerates, thereby obtaining a first raw material composition. The compounding ratio of each component here was calculated from the ratio of silicon to aluminum (Si / Al ratio) in the first raw material composition, and was expressed as the general formula of β-type Sialon: Si 12-a Al a O b N 16-b The values of a and b in the above formula are designed to be a=b=0.5.
[0063] 200 g of the obtained first raw material composition was filled into a cylindrical boron nitride container with a lid and an inner diameter of 10 cm and a height of 10 cm. The container was then placed in a carbon heater electric furnace and subjected to a heat treatment at 1950 °C for 10 hours in a pressurized nitrogen atmosphere of 0.8 MPa to obtain a first fired product. The first fired product was pulverized once using a supersonic jet pulverizer (manufactured by Nippon Pneumatic Mfg. Co., Ltd., product name "Supersonic Jet Pulverizer PJM-80SP") under conditions of an air pressure of 0.5 MPa and a feed rate of the first fired product of 3.0 kg / h. The pulverized first fired product was passed through a nylon sieve with a mesh size of 45 μm to obtain a β-sialon powder (D50: approximately 16 μm) to be used as a nucleating agent.
[0064] [Production of phosphor powder] Example 1 Using a micro V-shaped mixer (S-3 model, manufactured by Tsutsui Scientific Instruments Co., Ltd.), 93.29 mass% of α-type silicon nitride powder, 2.82 mass% of aluminum nitride powder, 0.91 mass% of aluminum oxide powder, 0.98 mass% of europium oxide powder, and 2.00 mass% of the nucleating agent (β-type sialon powder) prepared by the method described above were mixed. The resulting mixture was passed through a sieve with 250 μm openings to remove agglomerates, thereby obtaining a second raw material composition.
[0065] 200 g of the obtained second raw material composition was filled into a lidded cylindrical boron nitride container with an inner diameter of 10 cm and a height of 10 cm. Thereafter, this container was placed in an electric furnace of a carbon heater and subjected to a heat treatment (sintering process) at 1950 ° C for 10 hours in a pressurized nitrogen atmosphere of 0.8 MPa to obtain a second fired product. The second fired product was pulverized twice using a supersonic jet pulverizer (manufactured by Nippon Pneumatic Mfg. Co., Ltd., product name "Supersonic Jet Pulverizer PJM-80SP") under conditions of an air pressure of 0.5 MPa and a feed rate of the second fired product of 3.0 kg / h. The resulting mixture was then passed through a nylon sieve with a mesh size of 45 μm to obtain a fired powder.
[0066] 20 g of the resulting fired powder was packed into a lidded cylindrical boron nitride container with an inner diameter of 5 cm and a height of 3.5 cm. The container was then placed in a carbon heater electric furnace and heated at 1500 °C for 8 hours in an argon atmosphere at atmospheric pressure to obtain an annealed product. The annealed product was added to a mixed acid of hydrofluoric acid (concentration: 50% by mass) and nitric acid (concentration: 70% by mass) (a 1:1 volumetric mixture of hydrofluoric acid and nitric acid), and the resulting mixture was stirred at 75 °C for 30 minutes to perform an acid treatment. After the acid treatment, stirring was stopped to allow the powder to settle, and the supernatant and any fine particles contained therein were removed. Decantation was then repeated until the solution pH reached 5 or higher and the supernatant was clear. Decantation was performed by calculating the sedimentation time of the phosphor powder using the Stokes equation to remove fine particles with a particle diameter of 7 μm or less, and removing the supernatant above a predetermined height after a predetermined time had elapsed since the start of sedimentation. The dispersion medium was an aqueous solution of ion-exchanged water mixed with 0.05% by mass of sodium hexametaphosphate. The powder finally obtained as a precipitate was collected by filtration and dried to obtain a dry powder. Analysis of the dry powder using an oxygen / nitrogen analyzer and an ICP emission spectrometer revealed that the dry powder contained Si. 11.7 Al 0.3 O 0.3 N 15.7 :Eu 0.03 The dry powder was used as the phosphor powder of Example 1.
[0067] <Examples 2 to 4 and Comparative Examples 1 to 3> Phosphor powders of Examples 2 to 4 and Comparative Examples 1 to 3 were obtained in the same manner as in Example 1, except that the blending amounts of each component in the second raw material composition and the number of times the second fired product was pulverized were changed as shown in Table 1 below. As a result of analysis using an oxygen / nitrogen analyzer and an ICP optical emission analyzer, it was found that the phosphor powders of Examples 2 to 4 and Comparative Examples 1 to 3 contained Si 12-a Al a O b N 16-b :Eu x It was confirmed that the composition was (0.25≦a≦0.35, 0.25≦b≦0.35, 0.02≦x≦0.04).
[0068]
[0069] [Evaluation] The produced phosphor powders were evaluated as follows. The results are shown in Table 2.
[0070] <10% Cumulative Diameter (D10), 50% Cumulative Diameter (D50), and 90% Cumulative Diameter (D90)> The particle size distribution of each phosphor powder was measured in accordance with the particle size distribution measurement method by laser diffraction / scattering described in JIS R 1629:1997, "Method for measuring particle size distribution of fine ceramic raw materials by laser diffraction / scattering." Specifically, 0.03 g of the phosphor powder to be measured was first added to 100 mL of ion-exchanged water containing 0.05% by mass of sodium hexametaphosphate, and the mixture was dispersed for 3 minutes using an ultrasonic homogenizer (manufactured by Nippon Seiki Seisakusho Co., Ltd., product name "Ultrasonic Homogenizer US-150E," amplitude: 100%, oscillation frequency: 19.5 kHz, tip size: φ20, amplitude: 32±2 μm) to prepare a measurement sample. Thereafter, the particle size was measured using a particle size distribution measuring device (manufactured by Microtrac Bell Corporation, product name "Microtrac MT3300EX II"). From the obtained particle size distribution, D10, D50, and D90 were determined. Furthermore, based on the determined D10, D50, and D90 values, (D90-D10) / D50 (span value) was calculated.
[0071] <Emission Peak Intensity and Emission Peak Wavelength> The phosphor powder to be measured was filled into a concave cell so that the surface was smooth, and the cell was attached to the opening of an integrating sphere. Monochromatic light, separated into 455 nm wavelengths from a Xe lamp (light source), was introduced into the integrating sphere using an optical fiber as excitation light. This excitation light was irradiated onto the phosphor powder to be measured, and the fluorescence spectrum was measured. A spectrophotometer (manufactured by Otsuka Electronics Co., Ltd., product name "MCPD-7000") was used for the measurement. In the obtained fluorescence spectrum data, the wavelength showing the highest intensity in the wavelength range from 465 nm to 800 nm was determined as the emission peak wavelength. In addition, the emission peak intensity (%) was calculated as the relative value of the emission intensity value at the emission peak wavelength, when the emission intensity value at the emission peak wavelength determined for the phosphor powder of Comparative Example 1 was used as the reference.
[0072] <Chromaticity> From the data of the fluorescence spectrum measured by the above-described method in the wavelength range of 465 to 780 nm, the CIE chromaticity coordinate x value (chromaticity X) and y value (chromaticity Y) in the XYZ color system defined in JIS Z8781-3:2016 were calculated in accordance with JIS Z8724:2015.
[0073] When a standard sample of a β-sialon phosphor (NIMS Standard Green lot No. NSG1301, manufactured by SiAlON Corporation) was measured for emission peak wavelength, chromaticity X, and chromaticity Y in accordance with the above-mentioned measurement method, the peak wavelength was 543 nm, the chromaticity X was 0.356, and the chromaticity Y was 0.624.
[0074] The measured values of the emission peak wavelength, chromaticity X, and chromaticity Y may vary if the manufacturer of the measuring device, the production lot number, etc., changes. Therefore, the values measured by the measurement method described in this specification are used as the various measured values. However, when the manufacturer of the measuring device, the production lot number, etc., is changed, the measured values can also be corrected using the measured values of the standard sample of the β-sialon phosphor described above as the reference value.
[0075] <Relative Value of Total Luminous Flux of Light-Emitting Device> First, light-emitting devices (LED packages) of Examples 1 to 4 and Comparative Examples 1 to 3 were manufactured using the phosphor powders of Examples 1 to 4 and Comparative Examples 1 to 3, respectively. The phosphor powder and silicone resin (manufactured by Toray Dow Corning Co., Ltd., product name "OE6656") were weighed out so that the phosphor powder accounted for 2 mass% of the total amount of the phosphor powder and silicone resin, and mixed using a rotation-revolution mixer (manufactured by Thinky Corporation, product name "Awatori Rentaro (registered trademark) ARE-310"). Next, an LED was placed at the bottom of the recessed package body, and the LED was wire-bonded to the electrodes on the substrate. The LED was then mounted by injecting the mixture of the phosphor powder and silicone resin from a microsyringe. The resin was then cured at 120°C, followed by post-curing at 110°C for 10 hours and sealing to obtain a light-emitting device. The LEDs used had a peak emission wavelength of 448 nm and chip dimensions of 1.0 mm x 0.5 mm. The amount of phosphor powder relative to the total amount of phosphor powder and silicone resin was changed to 4 mass%, 8 mass%, and 16 mass%, but the rest of the light-emitting devices were obtained in the same manner. Using the above method, four types of light-emitting devices with different phosphor powder contents were manufactured for each example and comparative example.
[0076] The total luminous flux and chromaticity Y of the fabricated light-emitting devices were measured using a total luminous flux meter (a device manufactured by Otsuka Electronics Co., Ltd., combining a 500 mm diameter integrating hemisphere and a spectrophotometer (product name "MCPD-9800")). In order to compare the results of the light-emitting devices of each example and comparative example, the relative value of the total luminous flux was calculated as follows. First, for each example and comparative example, a graph was created based on the measurement results of four types of light-emitting devices, with the horizontal axis representing chromaticity Y and the vertical axis representing total luminous flux, to obtain an approximate curve. Based on the relational expression of the approximate curve, the total luminous flux when chromaticity Y = 0.230 was calculated. Next, the total luminous flux value of the light-emitting devices of each example and comparative example was calculated as a relative value (%) of the total luminous flux of the light-emitting device, assuming the value of the total luminous flux of the light-emitting device of Comparative Example 1 to be 100.0%.
[0077] <Variation in chromaticity Y of light-emitting device> The concentration of the phosphor powder was fixed at 8 mass%, and 20 light-emitting devices for each example and comparative example were fabricated using the method described above. The chromaticity Y of each fabricated light-emitting device was measured using the method described above, and the standard deviation of the chromaticity Y of the light-emitting device was calculated for each of Examples 1 to 4 and Comparative Examples 1 to 3. Furthermore, when the standard deviation of the chromaticity Y of the light-emitting device of Comparative Example 1 was set to 100%, the relative value (%) of the standard deviation for each example and comparative example was calculated as the variation in chromaticity Y of the light-emitting device.
[0078]
[0079] 10...substrate, 20...metal layer, 30...reflective portion, 40...light-emitting element, 42...die bond material, 44...bonding wire, 52...phosphor powder containing particles of europium-activated β-sialon phosphor, 54...other phosphor powder, 60...transparent sealing resin, 100...light-emitting device
Claims
1. A phosphor powder containing particles of a europium-activated β-sialon phosphor, in which, when the 10% cumulative diameter, 50% cumulative diameter, and 90% cumulative diameter in a volume-based cumulative particle size distribution are D10, D50, and D90, respectively, D50 is greater than 20.0 μm and not greater than 30.0 μm, and (D90-D10) / D50 is less than 1.
10.
2. The phosphor powder according to claim 1, wherein the europium-activated β-type sialon phosphor has a composition represented by the following general formula (1): Si 12-a A a O b N 16-b :Eu x ... (1) [In general formula (1), a, b, and x respectively represent values satisfying 0<a≦3, 0<b≦3, and 0<x≦0.1.] 3. A light emitting device comprising a light emitting element that emits primary light, and a wavelength converter that absorbs a portion of the primary light and emits secondary light having a wavelength longer than that of the primary light, wherein the wavelength converter contains the phosphor powder according to claim 1 or 2.
Citation Information
Patent Citations
β-TYPE SIALON PHOSPHOR AND LIGHT-EMITTING DEVICE
JP2020084177A
Phosphor and light emitting device
WO2017122800A1
Α-sialon fluorescent body and light-emitting device
WO2019188630A1
Β-sialon fluorescent body and light-emitting device
WO2019188631A1
Β-type sialon phosphor and light emitting device
WO2020105456A1