Production method for adhesive sheet, production method for optical film with adhesive sheet, and production method for image display device

The use of LEDs to cure pressure-sensitive adhesive sheets at 325-350 nm wavelength addresses inefficiencies in existing methods by reducing photopolymerization initiator residue and energy consumption, resulting in a more environmentally friendly and efficient adhesive sheet production process.

WO2024203364A1PCT designated stage expired Publication Date: 2024-10-03NITTO DENKO CORP

Patent Information

Application Number
PCT/JP2024/009900
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-13
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

The existing methods for manufacturing pressure-sensitive adhesive sheets, such as the thermosetting method, result in high energy consumption and significant CO2 emissions, and the photocuring method using black light sources leaves a large amount of photopolymerization initiator in the adhesive sheet, which is inefficient and environmentally impactful.

Method used

A method using light-emitting diodes (LEDs) to irradiate a coating layer with light in the wavelength range of 325 nm to 350 nm to form a pressure-sensitive adhesive sheet, reducing the amount of photopolymerization initiator residue and increasing the polymerization rate, while minimizing energy consumption and environmental impact.

Benefits of technology

This method efficiently produces adhesive sheets with reduced photopolymerization initiator residue, higher polymerization rates, and lower environmental impact, making it suitable for manufacturing pressure-sensitive adhesive sheets for optical films and image display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024009900_03102024_PF_FP_ABST
    Figure JP2024009900_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a new production method suitable for efficiently manufacturing an adhesive sheet. This production method for an adhesive sheet 1 includes a step for forming the adhesive sheet 1 by irradiating a coating layer 12 containing a photocurable composition with light 14 from a light-emitting diode 34. The peak wavelength of the light 14 irradiated onto the coating layer 12 is 325 nm to 350 nm. This production method for an optical film 21 with an adhesive sheet includes arranging an optical film 2 on an exposed surface 18 of the adhesive sheet 1 formed by the abovementioned production method to form the optical film 21 with an adhesive sheet.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing adhesive sheet, method for manufacturing optical film with adhesive sheet, and method for manufacturing image display device

[0001] The present invention relates to a method for producing a pressure-sensitive adhesive sheet, a method for producing an optical film with a pressure-sensitive adhesive sheet, and a method for producing an image display device.

[0002] Various image display devices, such as liquid crystal display devices and electroluminescence (EL) display devices, generally include an optical laminate including an optical film such as a polarizing film and an adhesive sheet. An adhesive sheet is typically used to bond the optical films included in the optical laminate or to bond the optical laminate to an image display panel. A typical adhesive sheet is a sheet obtained by polymerizing and crosslinking a monomer group including an acrylic monomer, a silicone monomer, or the like to harden the monomer group.

[0003] Patent Document 1 discloses an example of a pressure-sensitive adhesive sheet, which is produced by irradiating a coating layer of a pressure-sensitive adhesive composition disposed between two release liners with light.

[0004] Patent No. 6688054

[0005] A typical PSA sheet is manufactured, for example, by the following thermal curing method. First, a polymer produced by polymerizing a polymerizable monomer in an organic solvent is blended with a crosslinking agent or the like to prepare a PSA composition. This PSA composition is applied to a substrate such as a release liner, and the organic solvent is removed by heating to form a sheet. If necessary, heat aging is performed to complete the crosslinking, thereby producing a PSA sheet. This manufacturing process requires the combustion of a large amount of fuel, such as LNG, to generate the thermal energy required for the thermal removal of the solvent and for heat aging. Furthermore, releasing the thermally removed organic solvent directly into the atmosphere can have a significant adverse effect on the surrounding environment. Therefore, the organic solvent is often burned in a deodorizing furnace or the like before being released. In this case, not only is additional fuel required for combustion in the deodorizing furnace, but the organic solvent itself is also converted to CO2 by combustion and released into the atmosphere, resulting in a manufacturing process with extremely large CO2 emissions.

[0006] In recent years, climate change caused by greenhouse gases has become an urgent issue, and governments around the world are working to reduce CO2 emissions by setting numerical targets. In the manufacture of adhesive sheets, too, there is a demand for manufacturing processes that do not use organic solvents and that emit less CO2.

[0007] A method for producing a pressure-sensitive adhesive sheet using light (photocuring method) can reduce the amount of energy required to form the pressure-sensitive adhesive sheet and CO2 emissions compared to the above-mentioned thermal curing method. The photocuring method uses, for example, a black light source (Patent Document 1). However, according to the inventors' studies, a photocuring method using a black light source tends to leave a large amount of photopolymerization initiator remaining in the pressure-sensitive adhesive sheet produced, and there is room for improvement from the perspective of efficiently producing pressure-sensitive adhesive sheets.

[0008] Therefore, an object of the present invention is to provide a new production method suitable for efficiently producing a pressure-sensitive adhesive sheet.

[0009] The present invention provides a method for producing a pressure-sensitive adhesive sheet, comprising the step of irradiating a coating layer containing a photocurable composition with light from a light-emitting diode to form a pressure-sensitive adhesive sheet, wherein the light irradiated onto the coating layer has a peak wavelength of 325 nm to 350 nm.

[0010] The present invention further provides a method for producing an optical film with a pressure-sensitive adhesive sheet, comprising arranging an optical film on the exposed surface of the pressure-sensitive adhesive sheet formed by the above-mentioned production method to form an optical film with a pressure-sensitive adhesive sheet.

[0011] The present invention further provides a method for producing an image display device, which comprises bonding an optical film with a pressure-sensitive adhesive sheet formed by the above-mentioned production method to an image display panel to form an image display device.

[0012] According to the present invention, a new manufacturing method suitable for efficiently producing a pressure-sensitive adhesive sheet can be provided.

[0013] FIG. 1 is a schematic diagram illustrating an example of a method for producing a pressure-sensitive adhesive sheet of the present invention. FIG. 2 is a schematic diagram illustrating an example of a method for producing a pressure-sensitive adhesive sheet of the present invention. FIG. 3 is a schematic diagram illustrating an example of a method for producing a pressure-sensitive adhesive sheet of the present invention. FIG. 4 is a schematic diagram illustrating an example of a method for producing an optical film with a pressure-sensitive adhesive sheet of the present invention. FIG. 5 is a schematic diagram illustrating an example of a method for producing an optical film with a pressure-sensitive adhesive sheet of the present invention.

[0014] A method for producing a pressure-sensitive adhesive sheet according to a first aspect of the present invention includes a step of irradiating a coating layer containing a photocurable composition with light from a light-emitting diode to form a pressure-sensitive adhesive sheet, wherein the peak wavelength of the light irradiated onto the coating layer is 325 nm to 350 nm.

[0015] In a second aspect of the present invention, for example, in the manufacturing method according to the first aspect, the peak wavelength is 340±10 nm.

[0016] In a third aspect of the present invention, for example, in the manufacturing method according to the first or second aspect, the illuminance of the light irradiated onto the coating layer is 2.0 to 30 mW / cm 2 is.

[0017] In a fourth aspect of the present invention, for example, in the manufacturing method according to any one of the first to third aspects, the light is irradiated onto a laminate including a substrate sheet, the coating layer, and a release liner in this order.

[0018] In a fifth aspect of the present invention, for example, in the manufacturing method according to any one of the first to fourth aspects, the time for irradiating the coating layer with the light is 10 seconds to 1000 seconds.

[0019] In a sixth aspect of the present invention, for example, in the manufacturing method according to any one of the first to fifth aspects, the temperature of the coating layer is maintained at 10°C to 30°C while the coating layer is irradiated with the light.

[0020] In a seventh aspect of the present invention, for example, in the manufacturing method according to any one of the first to sixth aspects, the coating layer is irradiated with the light in an atmosphere having an oxygen concentration of 500 vol ppm or less.

[0021] In an eighth aspect of the present invention, for example, in the production method according to any one of the first to seventh aspects, the photocurable composition contains a monomer group including a (meth)acrylic monomer and / or a partial polymer of the monomer group.

[0022] In a ninth aspect of the present invention, for example, in the production method according to the eighth aspect, the polymerization rate of the monomer group in the pressure-sensitive adhesive sheet is 80% or more.

[0023] In a tenth aspect of the present invention, for example, in the production method according to the eighth or ninth aspect, the photocurable composition contains a photopolymerization initiator, and the amount of the photopolymerization initiator blended is 1.0 part by weight or less per 100 parts by weight of the total of the monomer group and the partially polymerized product.

[0024] In an eleventh aspect of the present invention, for example, in the manufacturing method according to the tenth aspect, the content of the photopolymerization initiator in the pressure-sensitive adhesive sheet is 500 wtppm or less.

[0025] In a twelfth aspect of the present invention, for example, in the production method according to any one of the first to eleventh aspects, the content of the solvent in the photocurable composition is 5% by weight or less.

[0026] A method for producing an optical film with a pressure-sensitive adhesive sheet according to a thirteenth aspect of the present invention includes forming an optical film with a pressure-sensitive adhesive sheet by arranging an optical film on an exposed surface of the pressure-sensitive adhesive sheet formed by the production method according to any one of the first to twelfth aspects.

[0027] In a fourteenth aspect of the present invention, for example, in the production method according to the thirteenth aspect, the optical film includes at least one film selected from the group consisting of a polarizing film and a retardation film.

[0028] A method for manufacturing an image display device according to a fifteenth aspect of the present invention includes bonding an optical film with a pressure-sensitive adhesive sheet formed by the manufacturing method according to the thirteenth or fourteenth aspect to an image display panel to form an image display device.

[0029] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be implemented in any modified form without departing from the gist of the present invention.

[0030] [Embodiment of Method for Producing Pressure-Sensitive Adhesive Sheet] As shown in Figure 1, the method for producing a pressure-sensitive adhesive sheet 1 of this embodiment includes a step of irradiating a coating layer 12 containing a photocurable composition with light 14 from a light-emitting diode (LED) 34 to form the pressure-sensitive adhesive sheet 1. In this step, the peak wavelength of the light 14 irradiated onto the coating layer 12 is 325 nm to 350 nm. The illuminance of this light 14 is preferably 2.0 to 30 mW / cm. 2 is.

[0031] In the manufacturing method of this embodiment, by using the above-mentioned light 14, the amount of remaining photopolymerization initiator in the formed pressure-sensitive adhesive sheet 1 tends to be reduced compared to when a black light source is used. Furthermore, according to studies by the present inventors, when the above-mentioned light 14 is used, the polymerization rate of the monomer group in the pressure-sensitive adhesive sheet 1 tends to be higher compared to when, for example, an LED that emits light with a peak wavelength of about 365 nm is used. In this way, the manufacturing method of this embodiment is suitable for efficiently producing the pressure-sensitive adhesive sheet 1.

[0032] As described above, the manufacturing method of this embodiment utilizes light 14 from an LED. Compared to black light sources, LEDs not only allow for easier adjustment of illuminance, but also tend to have a longer light source life. Compared to black light sources that use mercury, LEDs are also superior in terms of reducing environmental impact. Furthermore, according to the inventors' studies, LEDs emitting light 14 with a peak wavelength of 325 nm to 350 nm tend to generate less heat and make it easier to control the temperature of the coating layer 12 compared to LEDs emitting light with a peak wavelength of approximately 365 nm. Light 14 with a peak wavelength of 325 nm to 350 nm also tends to be more compatible with the absorption wavelength of photopolymerization initiators compared to light with a peak wavelength of approximately 365 nm. To the inventors' knowledge, no examples of adhesive sheets being produced using LEDs emitting light with a peak wavelength of 325 nm to 350 nm have been reported.

[0033] Specifically, the manufacturing method of this embodiment can be carried out by the following method. First, a laminate (first laminate) 10 is prepared, which includes, in this order, a base sheet 11, a coating layer 12 containing a photocurable composition, and a release liner 13. Light 14 is irradiated onto the first laminate 10. Irradiation with light 14 is typically carried out from the side of the base sheet 11. At this time, the light 14 passes through the base sheet 11 and reaches the coating layer 12, curing the coating layer 12. However, irradiation with light 14 may also be carried out from the side of the release liner 13, or from both the side of the release liner 13 and the side of the base sheet 11.

[0034] The formed PSA sheet 1 is sandwiched between the base sheet 11 and the release liner 13 until the release liner 13 is peeled off, and constitutes part of the second laminate 17. By peeling the release liner 13 off from the second laminate 17, a third laminate 15 including the base sheet 11 and the PSA sheet 1 is obtained. In the third laminate 15, the surface of the PSA sheet 1 is exposed to the outside.

[0035] As described above, the peak wavelength of the light 14 irradiated onto the first laminate 10 (specifically, the coating layer 12) is 325 nm to 350 nm. The peak wavelength of the light 14 is preferably 340±10 nm (330 nm to 350 nm), and may be 340±5 nm (335 nm to 345 nm), 340±2 nm (338 nm to 342 nm), or 340 nm. The peak wavelength refers to the wavelength at which the intensity of the light 14 reaches a maximum value in a spectrum showing the relationship between the wavelength and intensity of the light 14. The light 14 may further have a peak wavelength in a wavelength range other than 325 nm to 350 nm, but preferably does not have such a peak wavelength.

[0036] As described above, the illuminance of the light 14 irradiated onto the first laminate 10 (specifically, the coating layer 12) is preferably 2.0 to 30 mW / cm 2 The illuminance of the light 14 is 2.0 mW / cm 2 By setting the illuminance of the light 14 at 30 mW / cm or more, the coating layer 12 tends to be uniformly cured. 2When the irradiance of the light 14 is 30 mW / cm or less, the cleavage rate of the photopolymerization initiator contained in the photocurable composition can be appropriately adjusted, and the polymerization rate of the monomer group tends to increase. 2 When the temperature is less than 100°C, rapid heat generation in the coating layer 12 is suppressed, and there is a tendency for defects in the appearance of the PSA sheet 1 to be less likely to occur. When light 14 is irradiated from both the release liner 13 and base sheet 11 sides, the total illuminance of light 14 from the release liner 13 side and the illuminance of light 14 from the base sheet 11 side should be 2.0 to 30 mW / cm. 2 It is preferable that the temperature is adjusted to

[0037] The illuminance of the light 14 is preferably 2.5 mW / cm 2 or more, and 2 Above, 3.5mW / cm 2 Above, 4.0mW / cm 2 Above, 5.0mW / cm 2 Above, 6.0mW / cm 2 Above, 7.0mW / cm 2 Above, 8.0mW / cm 2 Above, 9.0mW / cm 2 or more, and even 10 mW / cm 2 The upper limit of the illuminance of the light 14 is, for example, 25 mW / cm 2 less than 20 mW / cm 2 Below 15mW / cm 2 The illuminance of the light 14 can be adjusted not only by controlling the LED 34 itself, but also by changing the distance between the LED 34 and the first laminate 10 .

[0038] The time for which the first laminate 10 (specifically, the coating layer 12) is irradiated with light 14 is not particularly limited and may be, for example, 10 to 1000 seconds, and may be 60 seconds or more, 100 seconds or more, 150 seconds or more, 200 seconds or more, or even 250 seconds or more. The upper limit of the time for irradiating with light 14 is, for example, 800 seconds or less, and in some cases may be 600 seconds or less. Irradiation with light 14 may be continuous or intermittent.

[0039] The integrated light amount of the light 14 on the first laminate 10 (specifically, the coating layer 12) is, for example, 25 mJ / cm 2 or more, and 100 mJ / cm 2 Above, 500mJ / cm 2 Above, 1000mJ / cm 2 Above, 2000mJ / cm 2 or more, and even 3000 mJ / cm 2 The upper limit of the integrated light amount of the light 14 is not particularly limited, and may be, for example, 30,000 mJ / cm. 2 or less, and 10,000 mJ / cm 2 Below 5000 mJ / cm 2 It may be the following:

[0040] While the first laminate 10 (specifically, the coating layer 12) is irradiated with light 14, the temperature of the coating layer 12 is maintained at, for example, 50° C. or less, preferably 10° C. to 30° C. In this case, the curing speed of the coating layer 12 is appropriately adjusted, and the number average molecular weight and weight average molecular weight of the polymer contained in the pressure-sensitive adhesive sheet 1 tend to increase.

[0041] In the manufacturing method of this embodiment, light 14 may be irradiated onto the first laminate 10 (specifically, the coating layer 12) in an atmosphere with a reduced oxygen concentration compared to the air (oxygen concentration 20.9 vol%). In this case, the curing of the coating layer 12 is less likely to be inhibited by oxygen, and the number-average molecular weight and weight-average molecular weight of the polymer contained in the pressure-sensitive adhesive sheet 1 tend to increase. Irradiation with light 14 may be performed in an atmosphere with an oxygen concentration of 20 vol% or less, 10 vol% or less, 1 vol% or less, 1000 vol ppm or less, or even 500 vol ppm or less. Irradiation with light 14 may also be performed in an atmosphere substantially free of oxygen. The atmosphere with a reduced oxygen concentration contains, for example, an inert gas such as argon or nitrogen, and is typically an inert gas atmosphere.

[0042] The manufacturing method of this embodiment may further include a heating step of heating the adhesive sheet 1 after irradiating with light 14. As an example, the heating step is performed on a third laminate 15 including the base sheet 11 and the adhesive sheet 1. The heating step promotes drying and curing of the adhesive sheet 1, and tends to further reduce the residual monomer contained in the adhesive sheet 1.

[0043] The conditions for the heating step are not particularly limited and can be adjusted appropriately. For example, the temperature for the heating step is preferably 40 to 200°C, more preferably 50 to 180°C, and even more preferably 70 to 170°C. The time for the heating step is, for example, 5 seconds to 20 minutes, preferably 5 seconds to 10 minutes, and more preferably 10 seconds to 5 minutes.

[0044] (Photocurable Composition) In this embodiment, the photocurable composition is a pressure-sensitive adhesive composition that forms a pressure-sensitive adhesive sheet 1 from the coating layer 12 upon irradiation with light 14. The photocurable composition contains, for example, a monomer group including a (meth)acrylic monomer and / or a partial polymer of the monomer group. The content of the (meth)acrylic component, i.e., the (meth)acrylic monomer and its partial polymer, in the photocurable composition may be 50% by weight or more, 60% by weight or more, 70% by weight or more, or even 80% by weight or more. In this case, an acrylic pressure-sensitive adhesive sheet 1 composed primarily of a (meth)acrylic polymer and its crosslinked product can be formed. However, the photocurable composition is not limited to the above examples. In this specification, (meth)acrylic refers to acrylic and methacrylic. (Meth)acrylate refers to acrylate and methacrylate.

[0045] An example of the (meth)acrylic monomer is a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 20 carbon atoms on the side chain. The number of carbon atoms in the alkyl group may be 7 or less, 6 or less, 5 or less, or even 4 or less. The alkyl group may be linear or branched. Examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, n-hexyl (meth)acrylate, isohexyl (meth)acrylate, isoheptyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. acrylate, n-octyl(meth)acrylate, isooctyl(meth)acrylate, n-nonyl(meth)acrylate, isononyl(meth)acrylate, n-decyl(meth)acrylate, isodecyl(meth)acrylate, n-dodecyl(meth)acrylate (lauryl(meth)acrylate), n-tridecyl(meth)acrylate, n-tetradecyl(meth)acrylate, pentadecyl(meth)acrylate, hexadecyl(meth)acrylate, heptadecyl(meth)acrylate, and octadecyl(meth)acrylate. The (meth)acrylic acid alkyl ester may be n-butyl(meth)acrylate.

[0046] The content of the (meth)acrylic acid alkyl ester in the monomer group is, for example, 40% by weight or more, and may be 50% by weight or more, 60% by weight or more, 70% by weight or more, 80% by weight or more, 85% by weight or more, 90% by weight or more, or even 95% by weight or more. In calculating the content, the weight of the partially polymerized product is converted into the weight of each monomer before polymerization.

[0047] The monomer group may contain a carboxyl group-containing monomer. The carboxyl group-containing monomer may be a (meth)acrylic monomer; in other words, the (meth)acrylic monomer may contain a carboxyl group-containing monomer. Examples of carboxyl group-containing monomers include (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid. The content of the carboxyl group-containing monomer in the monomer group may be, for example, 10% by weight or less, 9% by weight or less, 8% by weight or less, 7% by weight or less, 6% by weight or less, 5.5% by weight or less, or even 5% by weight or less. The lower limit of the content may be, for example, 0.1% by weight or more, 0.5% by weight or more, or even 1% by weight or more. The monomer group may not contain a carboxyl group-containing monomer.

[0048] The monomer group may contain a hydroxy group-containing monomer. The hydroxy group-containing monomer may be a (meth)acrylic monomer, in other words, the (meth)acrylic monomer may contain a hydroxy group-containing monomer. The hydroxy group-containing monomer may contribute to improving the cohesive strength of the PSA sheet. Examples of hydroxy group-containing monomers are 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)-methyl acrylate. The hydroxy group-containing monomer is preferably 2-hydroxyethyl (meth)acrylate or 4-hydroxybutyl (meth)acrylate. The content of the hydroxy group-containing monomer in the monomer group is, for example, 10% by weight or less, and may be 5% by weight or less, 4% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, 0.8% by weight or less, 0.5% by weight or less, 0.3% by weight or less, 0.2% by weight or less, or even 0.1% by weight or less. The lower limit of the content may be, for example, 0.01% by weight or more, 0.03% by weight or more, or even 0.05% by weight or more. The monomer group may not contain a hydroxy group-containing monomer.

[0049] The monomer group may include a nitrogen atom-containing monomer. The nitrogen atom-containing monomer means a monomer having at least one nitrogen atom in the molecule (per molecule).

[0050] As the nitrogen atom-containing monomer, from the viewpoint of improving foaming and peeling resistance, N-vinyl cyclic amide, (meth)acrylamide, etc. are preferred. The nitrogen atom-containing monomer may be used alone or in combination of two or more kinds.

[0051] The N-vinyl cyclic amide is preferably one represented by the following formula (1):

[0052] In formula (1), R 1 is a divalent organic group, preferably a divalent saturated or unsaturated hydrocarbon group, and more preferably a divalent saturated hydrocarbon group (e.g., an alkylene group having 3 to 5 carbon atoms). 1 are directly bonded via a single bond to form a ring structure.

[0053] As the N-vinyl cyclic amide represented by formula (1), from the viewpoint of improving foaming and peeling resistance, N-vinyl-2-pyrrolidone (NVP), N-vinyl-2-piperidone, N-vinyl-2-caprolactam, N-vinyl-3-morpholinone, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, etc. are preferred, more preferably N-vinyl-2-pyrrolidone and N-vinyl-2-caprolactam, and even more preferably N-vinyl-2-pyrrolidone.

[0054] Examples of (meth)acrylamides include (meth)acrylamide, N-alkyl(meth)acrylamide, N,N-dialkyl(meth)acrylamide, etc. Examples of N-alkyl(meth)acrylamides include N-ethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-n-butyl(meth)acrylamide, N-octylacrylamide, etc. N-alkyl(meth)acrylamides also include (meth)acrylamides having an amino group, such as dimethylaminoethyl(meth)acrylamide, diethylaminoethyl(meth)acrylamide, and dimethylaminopropyl(meth)acrylamide.

[0055] Examples of N,N-dialkyl(meth)acrylamides include N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, N,N-di(n-butyl)(meth)acrylamide, and N,N-di(t-butyl)(meth)acrylamide.

[0056] (Meth)acrylamides also include, for example, various N-hydroxyalkyl(meth)acrylamides, such as N-methylol(meth)acrylamide, N-(2-hydroxyethyl)(meth)acrylamide, N-(2-hydroxypropyl)(meth)acrylamide, N-(1-hydroxypropyl)(meth)acrylamide, N-(3-hydroxypropyl)(meth)acrylamide, N-(2-hydroxybutyl)(meth)acrylamide, N-(3-hydroxybutyl)(meth)acrylamide, N-(4-hydroxybutyl)(meth)acrylamide, and N-methyl-N-2-hydroxyethyl(meth)acrylamide.

[0057] (Meth)acrylamides also include, for example, various N-alkoxyalkyl(meth)acrylamides, such as N-methoxymethyl(meth)acrylamide and N-butoxymethyl(meth)acrylamide.

[0058] Examples of nitrogen atom-containing monomers other than N-vinyl cyclic amides and (meth)acrylamides include amino group-containing monomers such as aminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, and t-butylaminoethyl (meth)acrylate; cyano group-containing monomers such as acrylonitrile and methacrylonitrile; (meth)acryloylmorpholine, N-vinylpiperazine, N-vinylpyrrole, N-vinylimidazole, N-vinylpyrazine, N-vinylmorpholine, N-vinylpyrazole, vinylpyridine, vinylpyrimidine, vinyloxazole, vinylisoxazole, vinylthiazole, vinylisothiazole, vinylpyridazine, (meth)acryloylpyrrolidone, (meth)acryloylpyrrolidine, (meth)acryloylpiperidine, N-methyl Examples of the monomer include heterocycle-containing monomers such as vinylpyrrolidone; maleimide-based monomers such as N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, and N-phenylmaleimide; itaconimide-based monomers such as N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-laurylitaconimide, and N-cyclohexylitaconimide; and imide group-containing monomers such as succinimide-based monomers such as N-(meth)acryloyloxymethylenesuccinimide, N-(meth)acryloyl-6-oxyhexamethylenesuccinimide, and N-(meth)acryloyl-8-oxyoctamethylenesuccinimide; and isocyanate group-containing monomers such as 2-(meth)acryloyloxyethylisocyanate.

[0059] The content of the nitrogen atom-containing monomer in the monomer group is, for example, 40% by weight or less, 35% by weight or less, or even 30% by weight or less. The lower limit of the content is, for example, 5% by weight or more, 7% by weight or more, or even 10% by weight or more. The monomer group may not contain a nitrogen atom-containing monomer.

[0060] In the photocurable composition, each of the above-mentioned monomers may be contained as a partial polymer. The partial polymer may be either a homopolymer or a copolymer. The partial polymer may appropriately increase the viscosity of the photocurable composition, thereby contributing to the stable formation of the coating layer 12.

[0061] The photocurable composition typically contains a photopolymerization initiator. An example of the photopolymerization initiator is a photoradical generator that generates radicals when exposed to light 14. The photopolymerization initiator may have an absorption coefficient for light with a wavelength of 340 nm of, for example, 0.1 L / (g cm) or more, 0.5 L / (g cm) or more, 1.0 L / (g cm) or more, 3.0 L / (g cm) or more, or even 5.0 L / (g cm) or more. The upper limit of this absorption coefficient is not particularly limited, and may be, for example, 50 L / (g cm) or less. The absorption coefficient of the photopolymerization initiator is a calculated value from the absorbance of a 0.01 mg / mL methanol solution measured with a visible-ultraviolet spectrophotometer using a quartz cell with a 1 cm optical path length.

[0062] Examples of the photopolymerization initiator include benzoin ethers such as benzoin methyl ether, benzoin isopropyl ether, and benzil dimethyl ketal; substituted benzoin ethers such as anisole methyl ether; substituted acetophenones such as 2,2-diethoxyacetophenone and 2,2-dimethoxy-2-phenylacetophenone; α-hydroxyalkylphenones such as 1-hydroxycyclohexyl-phenyl ketone, 2-hydroxy-2-methylpropiophenone, 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, and 2,2'-dihydroxy-2,2'-dimethyl-1,1'-[methylenebis(4,1-phenylene)]bis(propan-1-one); and substituted alpha alkyl phenones such as 2-methyl-2-hydroxypropiophenone. aromatic sulfonyl chlorides such as 2-naphthalenesulfonyl chloride; photoactive oximes such as 1-phenyl-1,1-propanedione-2-(o-ethoxycarbonyl)-oxime; benzophenone-based compounds such as benzophenone, benzoylbenzoic acid, methyl benzoylbenzoate, 4-phenylbenzophenone, hydroxybenzophenone, acrylated benzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, and 3,3',4,4'-tetra(t-butylperoxycarbonyl)benzophenone; thioxanthone-based compounds such as thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, isopropylthioxanthone, 2,4-diisopropylthioxanthone, and 2,4-diethylthioxanthone;2,4,6-trichloro-s-triazine, 2-phenyl-4,6-bis(trichloromethyl)-s-triazine, 2-(p-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(p-tolyl)-4,6-bis(trichloromethyl)-s-triazine, 2-piperonyl-4,6-bis(trichloromethyl)-s-triazine, 2,4-bis(trichloromethyl)-6-styryl-s-triazine, 2-(naphth-1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-methoxy-naphth-1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2,4-trichloromethyl-(piperonyl)-6-triazine, 2,4-trichloromethyl- triazine-based compounds such as (4'-methoxystyryl)-6-triazine; oxime ester-based compounds such as 1,2-octanedione, 1-[4-(phenylthio)-, 2-(O-benzoyloxime)], and O-(acetyl)-N-(1-phenyl-2-oxo-2-(4'-methoxy-naphthyl)ethylidene)hydroxylamine; phosphine-based compounds such as bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide and 2,4,6-trimethylbenzoyldiphenylphosphine oxide; quinone-based compounds such as 9,10-phenanthrenequinone, camphorquinone, and ethylanthraquinone; borate-based compounds; carbazole-based compounds; imidazole-based compounds; and titanocene-based compounds. The photocurable composition may contain one or more photopolymerization initiators. In particular, α-hydroxyalkylphenone tends to have high absorption of light with wavelengths of 325 nm to 350 nm, and is therefore suitable for the production method of this embodiment.

[0063] The amount of photopolymerization initiator in the photocurable composition is, for example, 20 parts by weight or less, and may be 10 parts by weight or less, 5.0 parts by weight or less, 3.0 parts by weight or less, 1.0 parts by weight or less, 0.5 parts by weight or less, or even 0.3 parts by weight or less, relative to 100 parts by weight of the total of the monomer group and its partial polymer. When the amount of photopolymerization initiator is 1.0 part by weight or less, the weight-average molecular weight of the polymer contained in the pressure-sensitive adhesive sheet 1 tends to be sufficiently high. The lower limit of the amount of photopolymerization initiator is, for example, 0.02 parts by weight or more, and may be 0.05 parts by weight or more, relative to 100 parts by weight of the total of the monomer group and its partial polymer.

[0064] The photocurable composition may contain a crosslinking agent. An example of the crosslinking agent is a polyfunctional monomer having two or more polymerizable functional groups in one molecule. The polyfunctional monomer may be a (meth)acrylic monomer. Examples of the polyfunctional monomer are a monomer having two or more C=C bonds in one molecule, and a monomer having one or more C=C bonds and one or more polymerizable functional groups such as epoxy groups, aziridine groups, oxazoline groups, hydrazine groups, methylol groups, etc. in one molecule. The polyfunctional monomer is preferably a monomer having two or more C=C bonds in one molecule.

[0065] Examples of the polyfunctional monomer include (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,2-ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol diacrylate (N Polyfunctional acrylates (e.g., ester compounds of polyhydric alcohols and (meth)acrylic acid) such as 1,12-dodecanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and tetramethylolmethane tri(meth)acrylate; allyl (meth)acrylate, vinyl (meth)acrylate, divinylbenzene, epoxy acrylate, polyester acrylate, urethane acrylate, butyl di(meth)acrylate, and hexyl di(meth)acrylate. The polyfunctional monomer is preferably a polyfunctional acrylate, and more preferably 1,9-nonanediol diacrylate, trimethylolpropane tri(meth)acrylate, hexanediol di(meth)acrylate, or dipentaerythritol hexa(meth)acrylate.

[0066] The amount of the crosslinking agent to be added varies depending on the molecular weight, the number of functional groups, etc., but may be, for example, 5 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, 1 part by weight or less, 0.5 parts by weight or less, or even 0.3 parts by weight or less, relative to 100 parts by weight of the total of the monomer group and its partial polymer. The lower limit of the amount to be added is, for example, 0.01 parts by weight or more, or may even be 0.05 parts by weight or more.

[0067] The photocurable composition may contain additives other than those described above. Examples of the additives include a chain transfer agent, a silane coupling agent, a viscosity modifier, a tackifier, a plasticizer, a softener, an antioxidant, a filler, a colorant, an antioxidant, a surfactant, an antistatic agent, and an ultraviolet absorber.

[0068] The solvent content in the photocurable composition is, for example, 5 wt% or less, and may be 4 wt% or less, 3 wt% or less, 2 wt% or less, 1 wt% or less, or even 0.5 wt% or less. The photocurable composition may be substantially free of solvent. "Substantially free of solvent" means that solvents derived from additives and the like are allowed in a content of, for example, 0.1 wt% or less, preferably 0.05 wt% or less, and more preferably 0.01 wt% or less.

[0069] The viscosity of the photocurable composition is preferably 1 to 100 poise. A photocurable composition having a viscosity in the above range is particularly suitable for forming the coating layer 12.

[0070] (Release Liner) An example of the substrate of the release liner 13 (hereinafter referred to as "liner substrate") is a resin film. Examples of resins that can be contained in the liner substrate include polyesters such as polyethylene terephthalate and polyethylene naphthalate, acetate resins, polyethersulfone, polycarbonate, polyamide, polyimide, polyolefin, (meth)acrylic resins, polyvinyl chloride, polyvinylidene chloride, polystyrene, polyvinyl alcohol, polyarylate, and polyphenylene sulfide. The resin is preferably a polyester such as polyethylene terephthalate.

[0071] The release liner 13 may be transparent to light 14. As an example, the spectral transmittance of the release liner 13 for light with a wavelength of 340 nm may be, for example, 60% or more, 70% or more, or even 80% or more. The upper limit of the spectral transmittance is not particularly limited and may be, for example, 95% or less, or 90% or less. The spectral transmittance for light with a wavelength of 340 nm can be determined from the spectrum obtained by measuring the total light transmittance spectrum of the release liner 13 in the wavelength range of 300 to 2000 nm using, for example, a commercially available spectrophotometer.

[0072] The thickness of the release liner 13 is, for example, 10 to 200 μm, and may be 25 to 150 μm.

[0073] The release liner 13 may include a layer other than the liner substrate. The release liner 13 may include a release layer. The release liner 13 includes, for example, a liner substrate and a release layer formed on one surface of the liner substrate. This release liner 13 can be used with the release layer facing the coating layer 12.

[0074] The release layer is typically a cured layer of a release agent composition containing a release agent. A variety of release agents can be used as the release agent, including silicone-based release agents, fluorine-based release agents, long-chain alkyl-based release agents, fatty acid amide-based release agents, and silica powder. The release liner 13 may be provided with a cured layer of a release agent composition containing a silicone-based release agent as the main component (hereinafter referred to as the "silicone release layer"). A silicone release layer is particularly suitable for achieving both good adhesion to the PSA sheet 1 and good releasability. In this specification, the term "main component" refers to the component with the highest content.

[0075] Silicone-based release agents are various curable silicone materials such as addition reaction type, condensation reaction type, ultraviolet curable type, electron beam curable type, and solventless type, with addition reaction curable silicone materials being preferred. Addition reaction curable silicone materials are particularly suitable for forming a release layer that has both good adhesion and releasability to the pressure-sensitive adhesive sheet 1. The curable silicone material may be a silicone-modified resin in which reactive silicone is introduced into an organic resin such as a urethane, epoxy, or alkyd resin by graft polymerization or the like.

[0076] An example of an addition reaction curable silicone material is a polyorganosiloxane having a vinyl group or an alkenyl group in the molecule. The addition reaction curable silicone material may not have a hydrosilyl group. Examples of alkenyl groups include 3-butenyl, 4-pentenyl, 5-hexenyl, 6-heptenyl, 7-octenyl, 8-nonenyl, 9-decenyl, 10-undecenyl, and 11-dodecenyl groups. Examples of polyorganosiloxanes include polyalkylalkylsiloxanes such as polydimethylsiloxane, polydiethylsiloxane, and polymethylethylsiloxane, polyalkylarylsiloxanes, and copolymers of multiple Si atom-containing monomers such as poly(dimethylsiloxane-diethylsiloxane). The polyorganosiloxane is preferably polydimethylsiloxane.

[0077] A release agent composition containing a silicone-based release agent as a main component (hereinafter referred to as "silicone release agent composition") usually contains a crosslinking agent. An example of the crosslinking agent is a polyorganosiloxane having a hydrosilyl group. The crosslinking agent may have two or more hydrosilyl groups in one molecule.

[0078] The silicone release agent composition may contain a curing catalyst. An example of the curing catalyst is a platinum-based catalyst. Examples of the platinum-based catalyst are chloroplatinic acid, platinum olefin complexes, and chloroplatinic acid olefin complexes. The amount of the platinum-based catalyst used is, for example, 10 to 1,000 ppm (by weight, platinum equivalent) based on the total solids content of the composition.

[0079] The silicone release agent composition may contain additives. Examples of additives are release control agents and adhesion promoters. Examples of release control agents are unreactive silicone resins, and more specific examples are organosiloxanes such as octamethylcyclotetrasiloxane, and MQ resins. The amount of the release control agent and adhesion promoter used is, for example, 1 to 30% by weight in total, based on the total solids content of the composition. Further examples of additives are fillers, antistatic agents, antioxidants, UV absorbers, plasticizers, and colorants. The amount of the additional additives used is, for example, 10% by weight or less in total, based on the total solids content of the composition.

[0080] The silicone release agent composition may contain an organic solvent. Examples of organic solvents include hydrocarbon solvents such as cyclohexane, n-hexane, and n-heptane; aromatic solvents such as toluene and xylene; ester solvents such as ethyl acetate and methyl acetate; ketone solvents such as acetone and methyl ethyl ketone; and alcohol solvents such as methanol, ethanol, and butanol. Two or more organic solvents may be contained. The amount of organic solvent used is preferably 80 to 99.9% by weight of the silicone release agent composition.

[0081] The release layer can be formed, for example, by heating and drying a coating film containing the release agent composition formed on a liner substrate. Various coating methods can be used to apply the release agent composition, such as roll coating, kiss roll coating, gravure coating, reverse coating, roll brushing, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and die coating. For heating and drying, for example, hot air drying can be used. The heating temperature and time vary depending on the heat resistance of the liner substrate, but are typically 80 to 150°C and about 10 seconds to 10 minutes. If necessary, irradiation with active energy rays such as ultraviolet rays may be used in combination.

[0082] The thickness of the release layer is, for example, 10 to 300 nm. The upper limit of the thickness may be 200 nm or less, 150 nm or less, 120 nm or less, 110 nm or less, 100 nm or less, less than 100 nm, 90 nm or less, 80 nm or less, 70 nm or less, less than 70 nm, or even 65 nm or less. The lower limit of the thickness may be 15 nm or more, 20 nm or more, 25 nm or more, 30 nm or more, 35 nm or more, 40 nm or more, 45 nm or more, or even 50 nm or more.

[0083] The release liner 13 may be in the form of a sheet or a continuous piece.

[0084] (Base Sheet) An example of the base sheet 11 is a resin film. Examples of the resin contained in the base sheet 11 are the same as the examples of the resin that can be contained in the liner base material.

[0085] The base sheet 11 preferably has excellent transmittance to light 14. As an example, the spectral transmittance of the base sheet 11 for light with a wavelength of 340 nm is, for example, 60% or more, and may be 70% or more, or even 80% or more. The higher the spectral transmittance, the more efficiently the coating layer 12 can be cured by light 14. Furthermore, the base sheet 11 can be prevented from absorbing light 14 and generating heat. The upper limit of the spectral transmittance is not particularly limited, and may be, for example, 95% or less, or 90% or less. The spectral transmittance for light with a wavelength of 340 nm can be determined by the method described above for the release liner 13.

[0086] The thickness of the base sheet 11 is, for example, 10 to 200 μm, and may be 25 to 150 μm.

[0087] The base sheet 11 may have a release layer on the surface on the side of the coating layer 12. Examples of the release layer that the base sheet 11 may have and the manufacturing method thereof are the same as the examples of the release layer that the release liner 13 may have and the manufacturing method thereof. Both the release liner 13 and the base sheet 11 may have a release layer. In this case, both release layers may be formed from a release agent composition containing the same release agent as a main component. Furthermore, the thicknesses of both release layers may be different; for example, the release layer provided on the base sheet 11 may be thicker.

[0088] For the base sheet 11 , a sheet having a greater peel strength from the pressure-sensitive adhesive sheet 1 than the release liner 13 can usually be selected.

[0089] The base sheet 11 may be in the form of a sheet or a continuous sheet.

[0090] (First Laminate and Formation Thereof) The first laminate 10 may include an additional layer other than the base sheet 11, the coating layer 12, and the release liner 13. The additional layer may be disposed on the side of the base sheet 11 and / or the release liner 13 opposite to the side on which the coating layer 12 is disposed. The coating layer 12 is preferably in contact with the base sheet 11 and the release liner 13.

[0091] The first laminate 10 can be formed, for example, by forming a coating layer 12 on a base sheet 11 (or a release liner 13) and then placing the release liner 13 (or base sheet 11) on the formed coating layer 12. Alternatively, the first laminate 10 may be formed by applying the photocurable composition in a poured manner into the space between the base sheet 11 and the release liner 13, which are held at a predetermined distance so that their main surfaces face each other.

[0092] The coating layer 12 can be formed by various coating methods such as roll coating, kiss roll coating, gravure coating, reverse coating, roll brushing, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and die coating.

[0093] The thickness of the coating layer 12 can be adjusted depending on the desired thickness of the pressure-sensitive adhesive sheet 1, and may be, for example, 2 mm or less, 1 mm or less, 2 to 300 μm, 2 to 200 μm, 2 to 150 μm, 2 to 100 μm, 2 to 70 μm, 2 to 50 μm, 5 to 40 μm, 10 to 30 μm, 10 to 25 μm, or even 10 to 20 μm.

[0094] The first laminate 10 may include a long base sheet 11, a long coating layer 12, and a long release liner 13, or in other words, may be long. The long first laminate 10 can be obtained, for example, by forming the coating layer 12 between the base sheet 11 and the release liner 13 while conveying them after they have been unwound from a roll.

[0095] (Adhesive Sheet) As described above, the adhesive sheet 1 produced by the manufacturing method of this embodiment tends to have a low amount of residual photopolymerization initiator. Adhesive sheets 1 with a low amount of residual photopolymerization initiator tend to be less prone to yellowing and foaming in high-temperature environments. As an example, the content of the photopolymerization initiator in the adhesive sheet 1 is, for example, 500 wtppm or less, and may be 300 wtppm or less, 200 wtppm or less, 150 wtppm or less, 120 wtppm or less, 100 wtppm or less, 80 wtppm or less, 50 wtppm or less, or even 30 wtppm or less. The adhesive sheet 1 may be substantially free of photopolymerization initiator.

[0096] Furthermore, the pressure-sensitive adhesive sheet 1 produced by the manufacturing method of this embodiment tends to have a high polymerization rate of the monomer group and a low residual amount of the monomer group. A pressure-sensitive adhesive sheet 1 with a low residual amount of the monomer group not only contributes to improved productivity, but also tends to have a reduced odor. This pressure-sensitive adhesive sheet 1 also has the advantage of being easy to handle and transport. The polymerization rate of the monomer group in the pressure-sensitive adhesive sheet 1 is preferably 80% or more, and may be 85% or more, 90% or more, 95% or more, 97% or more, 98% or more, or even 99% or more.

[0097] According to the manufacturing method of this embodiment, the molecular weight of the polymer contained in the pressure-sensitive adhesive sheet 1 also tends to be large. For example, when the manufacturing method of this embodiment is performed using a sample having the same composition as the photocurable composition described above except that it does not contain a crosslinking agent, the weight-average molecular weight (Mw) of the polymer obtained by polymerization of the monomer group contained in the sample is, for example, 400,000 or more, 500,000 or more, 700,000 or more, 800,000 or more, 900,000 or more, or even 1,000,000 or more. The larger this Mw, the more likely peeling of the pressure-sensitive adhesive sheet 1 in high-temperature environments and the like is suppressed. The upper limit of Mw is not particularly limited, and is, for example, 3,000,000 or less. The number-average molecular weight (Mn) of the above polymer may be, for example, 80,000 or more, 100,000 or more, 150,000 or more, 180,000 or more, 200,000 or more, or even 250,000 or more. The upper limit of Mn is not particularly limited, and is, for example, 600,000 or less. The weight average molecular weight (Mw) / number average molecular weight (Mn), which indicates the molecular weight distribution, is, for example, 1.8 to 10, or may be 1.8 to 7, or even 1.8 to 5. The weight average molecular weight and number average molecular weight are determined from values ​​measured by GPC (gel permeation chromatography) and calculated in terms of polystyrene.

[0098] The gel fraction of the pressure-sensitive adhesive sheet 1 is, for example, 50% or more, and may be 75% or more, 80% or more, or even 85% or more.

[0099] The thickness of the pressure-sensitive adhesive sheet 1 is, for example, 2 mm or less, and may be 1 mm or less, 2 to 300 μm, 2 to 200 μm, 2 to 150 μm, 2 to 100 μm, 2 to 70 μm, 2 to 50 μm, 5 to 40 μm, 10 to 30 μm, 10 to 25 μm, or even 10 to 20 μm.

[0100] The pressure-sensitive adhesive sheet 1 produced by the manufacturing method of this embodiment is particularly suitable for applications requiring high light transmittance (for example, optical applications). However, the pressure-sensitive adhesive sheet 1 can also be used for various applications other than optical applications. The pressure-sensitive adhesive sheet 1 may also be used as a double-sided tape.

[0101] Next, another example of a method for producing a pressure-sensitive adhesive sheet will be described with reference to Figure 2. In this example, a coating layer 12 of a photocurable composition is formed on one side of a long substrate sheet 11 unwound from a roll 31 by a coating device 32. Next, a long release liner 13 unwound from a roll 33 is placed on top of the coating layer 12 to form a long first laminate 10. Next, light 14 is irradiated from an LED 34 onto the first laminate 10 to form a long pressure-sensitive adhesive sheet 1. Next, the release liner 13 is peeled from a second laminate 17 containing the pressure-sensitive adhesive sheet 1 and wound around a roll 35. The above steps are performed while the substrate sheet 11 and release liner 13 are being transported. The method of Figure 2 is particularly suitable for mass production of pressure-sensitive adhesive sheets.

[0102] Next, another example of a method for producing a PSA sheet will be described with reference to Figure 3. In this example, a photocurable composition is applied using an application device 32 between a long substrate sheet 11 unwound from a roll 31 and a long release liner 13 unwound from a roll 33. This forms a coating layer 12 containing the photocurable composition, and a long first laminate 10 is obtained.

[0103] Next, the first laminate 10 is transported so as to pass between the pair of light sources 38a and 38b. Specifically, the first laminate 10 first passes through a first region 40A near the light source 38a. Next, the first reversing mechanism (first conveying roller 39a) is used to reverse the movement direction of the first laminate 10, and the first laminate 10 is moved in the opposite direction to the movement direction in the first region 40A. This causes the first laminate 10 to pass through a second region 40B, which is closer to the light source 38b than the first region 40A. Next, the second reversing mechanism (second conveying roller 39b) is used to further reverse the movement direction of the first laminate 10, and the first laminate 10 is moved in the same direction as the movement direction in the first region 40A. This causes the first laminate 10 to pass through a third region 40C near the light source 38b.

[0104] The light source 38a is typically an LED that emits light L1 with a peak wavelength of 325 nm to 350 nm. Similarly, the light source 38b is typically an LED that emits light L2 with a peak wavelength of 325 nm to 350 nm. The above-mentioned LED 34 can be used as the light sources 38a and 38b.

[0105] In the example of FIG. 3, the sum of the illuminance of light L1 from the release liner 13 side and the illuminance of light L2 from the base sheet 11 side in the first region 40A (illuminance LA), the sum of the illuminance of light L1 from the base sheet 11 side and the illuminance of light L2 from the release liner 13 side in the second region 40B (illuminance LB), and the sum of the illuminance of light L1 from the release liner 13 side and the illuminance of light L2 from the base sheet 11 side in the third region 40C (illuminance LC) are each 2.0 to 30 mW / cm 2 It is preferable that the illuminances LA to LC are adjusted to be greater than the distance between the light source 38a and the first region 40A. The illuminances LA to LC may satisfy the relationship LA<LB<LC. The illuminances LA to LC can be adjusted by the positions and outputs of the light sources 38a and 38b. As an example, the distance between the light source 38a and the first region 40A may be adjusted to be greater than the distance between the light source 38b and the third region 40C.

[0106] By passing the light between a pair of light sources 38a and 38b, light L1 and L2 having a peak wavelength of 325 nm to 350 nm is irradiated onto the coating layer 12, forming a long adhesive sheet 1. Next, the release liner 13 is peeled from the second laminate 17 containing the adhesive sheet 1 and wound up into a roll 35. The method of Figure 3 allows the adhesive sheet to be formed in a small space, and is particularly suitable for mass production of adhesive sheets.

[0107] 3, it is preferable that the polymerization rate of the monomer group is 50% or more when the monomer group passes through the first region 40A. In this case, when the moving direction of the first laminate 10 is reversed using the first reversing mechanism (first conveying roller 39a), the components constituting the first laminate 10 tend to be less prone to appearance defects such as wrinkles, streaks, and lifting.

[0108] [Method for manufacturing an optical film with a pressure-sensitive adhesive sheet] An example of a method for manufacturing an optical film with a pressure-sensitive adhesive sheet of this embodiment will be described with reference to Figure 4. In the example of Figure 4, an optical film 2 is placed on exposed surface 18 of a pressure-sensitive adhesive sheet 1 formed by peeling off release liner 13 from second laminate 17 produced by the method described above, to form an optical film with a pressure-sensitive adhesive sheet 21. Note that, before placing the optical film 2, exposed surface 18 of pressure-sensitive adhesive sheet 1 may be subjected to a surface modification treatment.

[0109] The pressure-sensitive adhesive sheet-attached optical film 21 includes a base sheet 11, a pressure-sensitive adhesive sheet 1, and an optical film 2, in this order. The pressure-sensitive adhesive sheet-attached optical film 21 can be used in an image display device or the like, for example, as an optical laminate including the pressure-sensitive adhesive sheet 1 and the optical film 2, either as is or after the base sheet 11 has been peeled off. The optical laminate may be attached to an object (e.g., an image forming panel) via the pressure-sensitive adhesive sheet 1. However, the use of the pressure-sensitive adhesive sheet-attached optical film 21 is not limited to the above example. An additional member such as an optical film may be disposed on the exposed surface 18 formed by peeling off the base sheet 11 from the pressure-sensitive adhesive sheet-attached optical film 21. As an example, a pressure-sensitive adhesive sheet-attached optical film 22 can be formed, including an optical film 2A, a pressure-sensitive adhesive sheet 1, and an optical film 2B, in this order (see FIG. 5 ). The optical films 2A and 2B may be the same or different from each other.

[0110] The optical film 2 may be disposed directly or indirectly on the exposed surface 18. In other words, the optical film 2 may be disposed so as to be in contact with the exposed surface 18, or may be disposed with another layer sandwiched between the optical film 2 and the exposed surface 18.

[0111] Another example of the method for manufacturing a pressure-sensitive adhesive sheet-attached optical film of this embodiment will be described with reference to Figure 6. In this example, a long optical film 2 is placed on the exposed surface 18 of the pressure-sensitive adhesive sheet 1 in the third laminate 15 formed by the method of Figure 2, to form a long pressure-sensitive adhesive sheet-attached optical film 21. The optical film 2 is unwound from a roll 36 and placed on the exposed surface 18. As shown in Figure 6, the formation of the pressure-sensitive adhesive sheet 1 and the formation of the pressure-sensitive adhesive sheet-attached optical film 21 may be carried out continuously. The method of Figure 6 is particularly suitable for mass production of pressure-sensitive adhesive sheet-attached optical films 21.

[0112] The optical film 2 is, for example, a film including at least one selected from the group consisting of a polarizing film and a retardation film. The optical film 2 may be a laminated film including a polarizing film and / or a retardation film. The optical film 2 may include a glass film. However, the optical film 2 is not limited to the above examples.

[0113] The polarizing film includes a polarizer. The polarizing film typically includes a polarizer and a protective film (transparent protective film). The protective film is disposed, for example, in contact with a main surface (the surface having the largest area) of the polarizer. The polarizer may be disposed between two protective films. The protective film may be disposed on at least one surface of the polarizer.

[0114] The polarizer is not particularly limited, and examples thereof include a hydrophilic polymer film such as a polyvinyl alcohol film, a partially formalized polyvinyl alcohol film, or an ethylene-vinyl acetate copolymer partially saponified film, which has been uniaxially stretched after adsorbing a dichroic substance such as iodine or a dichroic dye; a polyene-based oriented film such as a dehydrated polyvinyl alcohol or a dehydrochlorinated polyvinyl chloride; etc. A polarizer typically comprises a polyvinyl alcohol film (polyvinyl alcohol films include an ethylene-vinyl acetate copolymer partially saponified film) and a dichroic substance such as iodine.

[0115] The thickness of the polarizer is not particularly limited and may be, for example, 80 μm or less, 50 μm or less, 30 μm or less, 25 μm or less, or even 20 μm or less. The lower limit of the polarizer thickness is not particularly limited and may be, for example, 1 μm or more, 5 μm or more, 10 μm or more, or even 15 μm or more. A thin polarizer (for example, a thickness of 20 μm or less) is suppressed in dimensional change and can contribute to improving the durability of the optical laminate, particularly durability at high temperatures.

[0116] The material for the protective film may be, for example, a thermoplastic resin having excellent transparency, mechanical strength, thermal stability, moisture-blocking properties, isotropy, etc. Specific examples of such thermoplastic resins include cellulose resins such as triacetyl cellulose, polyester resins, polyethersulfone resins, polysulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth)acrylic resins, cyclic polyolefin resins (norbornene-based resins), polyarylate resins, polystyrene resins, polyvinyl alcohol resins, and mixtures thereof. The material for the protective film may be a thermosetting resin or an ultraviolet-curable resin such as a (meth)acrylic, urethane, acrylic urethane, epoxy, or silicone-based resin. When the polarizing film has two protective films, the materials of the two protective films may be the same or different. For example, a protective film made of a thermoplastic resin may be bonded to one main surface of the polarizer via an adhesive, and a protective film made of a thermosetting resin or an ultraviolet-curable resin may be bonded to the other main surface of the polarizer. The protective film may contain one or more optional additives, such as ultraviolet absorbers, antioxidants, lubricants, plasticizers, release agents, color inhibitors, flame retardants, nucleating agents, antistatic agents, pigments, and colorants.

[0117] The thickness of the protective film can be determined as appropriate, but is generally about 10 to 200 μm in view of strength, workability such as handling, thinness, and the like.

[0118] The polarizer and the protective film are usually adhered to each other via an aqueous adhesive or the like. Examples of aqueous adhesives include isocyanate-based adhesives, polyvinyl alcohol-based adhesives, gelatin-based adhesives, vinyl latex, aqueous polyurethane, and aqueous polyester. Examples of adhesives other than the above-mentioned adhesives include ultraviolet-curable adhesives and electron beam-curable adhesives. Electron beam-curable polarizing plate adhesives exhibit suitable adhesive properties for various protective films. The adhesive may contain a metal compound filler.

[0119] In the polarizing film, a retardation film or the like can be formed on the polarizer instead of the protective film. Another protective film or a retardation film or the like can be further provided on the protective film.

[0120] The protective film may have a hard coat layer on the surface opposite to the surface bonded to the polarizer, and may also be subjected to treatments for purposes such as anti-reflection, anti-sticking, diffusion, and anti-glare.

[0121] The polarizing film may be a circular polarizing film.

[0122] The retardation film may be a film obtained by stretching a polymer film or a film obtained by aligning and fixing a liquid crystal material. The retardation film has birefringence, for example, in the in-plane and / or thickness direction.

[0123] The retardation film includes an anti-reflection retardation film (see JP 2012-133303 A,

[0221] ,

[0222] ,

[0228] ), a viewing angle compensation retardation film (see JP 2012-133303 A,

[0225] ,

[0226] ), an inclined orientation retardation film for viewing angle compensation (see JP 2012-133303 A,

[0227] ), and the like.

[0124] The specific structure of the retardation film, such as the retardation value, arrangement angle, three-dimensional birefringence, whether it is a single layer or a multilayer, is not particularly limited, and any known retardation film can be used.

[0125] The thickness of the retardation film is preferably 20 μm or less, more preferably 10 μm or less, still more preferably 1 to 9 μm, and particularly preferably 3 to 8 μm.

[0126] The retardation film may include, for example, a quarter-wave plate and / or a half-wave plate in which a liquid crystal material is aligned and fixed.

[0127] [Method for manufacturing an image display device] An image display device may be formed using the optical film with adhesive sheet formed by the above-mentioned manufacturing method. The image display device can be formed, for example, by bonding the optical film with adhesive sheet 21, 22 to an image display panel. The bonding may be performed using an adhesive sheet 1. The image display device may be an organic EL display or a liquid crystal display. However, the image display device is not limited to the above examples. The image display device may be an electroluminescence (EL) display, a plasma display (PD), a field emission display (FED), etc. The image display device can be used for home appliance applications, in-vehicle applications, public information displays (PID), etc.

[0128] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the examples shown below.

[0129] Monomer Syrup A1: 99 parts by weight of n-butyl acrylate (BA), 1 part by weight of 4-hydroxybutyl acrylate (HBA), 0.05 parts by weight of 1-hydroxycyclohexyl-phenyl ketone (Omnirad 184, manufactured by IGM Resins BV) as a photopolymerization initiator, and 0.05 parts by weight of 2,2-dimethoxy-1,2-diphenylethan-1-one (Omnirad 651, manufactured by IGM Resins BV) were placed in a four-neck flask and irradiated with ultraviolet light under a nitrogen atmosphere to obtain a partially photopolymerized monomer syrup A1. UV irradiation was continued until the viscosity of the liquid in the flask reached approximately 20 Pa s (measurement conditions: BH viscometer No. 5 rotor, 10 rpm, measurement temperature 30°C).

[0130] [Monomer Syrups A2 to A9] Monomer syrups A2 to A9 were prepared in the same manner as for Monomer Syrup A1, except that the monomers used were changed as shown in Table 1.

[0131]

[0132] The abbreviations in Table 1 are as follows: BA: n-butyl acrylate AA: acrylic acid HBA: 4-hydroxybutyl acrylate Omnirad 184: 1-hydroxycyclohexyl-phenyl ketone (Omnirad 184, manufactured by IGM Resins BV) Omnirad 651: 2,2-dimethoxy-1,2-diphenylethan-1-one (Omnirad 651, manufactured by IGM Resins BV) Omnirad 819: bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (Omnirad 819, manufactured by IGM Resins BV) Omnirad 127: 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)2-methylpropan-1-one (Omnirad 127, manufactured by IGM Resins BV) Omnirad 2959: 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone (Omnirad 2959, manufactured by IGM Resins BV)

[0133] [Photocurable Compositions C1 to C13] Next, the monomer syrup, the monomer, and the crosslinking agent were mixed so as to have the compositions shown in Table 2 below, thereby obtaining photocurable compositions C1 to C13.

[0134]

[0135] The abbreviations in Table 2 are as follows: AA: acrylic acid NVP: N-vinyl-2-pyrrolidone NDDA: 1,9-nonanediol diacrylate

[0136] The final compositions of the monomers contained in photocurable compositions C3 and C4 are shown in Table 3 below.

[0137]

[0138] The abbreviations in Table 3 are as follows: BA: n-butyl acrylate AA: acrylic acid HBA: 4-hydroxybutyl acrylate NVP: N-vinyl-2-pyrrolidone

[0139] Example 1 Preparation of Release Liner L1 A silicone-based release agent composition was obtained by mixing 30 parts by weight of an addition reaction curable silicone (LTC761 containing a hexenyl group-containing polyorganosiloxane, a 30 wt % toluene solution, manufactured by Dow Corning Toray), 0.9 parts by weight of a release control agent (BY24-850 containing an unreactive silicone resin, manufactured by Dow Corning Toray), and 2 parts by weight of a curing catalyst (SRX212 containing a platinum catalyst, manufactured by Dow Corning Toray), and a toluene / hexane mixed solvent (volume ratio 1:1) as a dilution solvent. The silicone solids concentration in the release agent composition was 1.0 wt %. Next, the release agent composition was applied with a wire bar to one side of a liner substrate (Lumirror XD500P, a polyester film, 75 μm thick), and heated at 130° C. for 1 minute to prepare a release liner L1 having a release layer (thickness 60 nm) on one side.

[0140] [Preparation of Pressure-Sensitive Adhesive Sheet] The photocurable composition C1 was applied to one side of a substrate sheet (Lumirror XD500P, a polyester film without a release layer, with a thickness of 75 μm) using an applicator to form a coating layer (thickness of 20 μm). Next, a release liner L1 was placed on the formed coating layer to obtain a first laminate. The release liner L1 was placed so that the release layer was in contact with the coating layer. Next, a light source with an illuminance of 4 mW / cm was applied from the substrate sheet side of the first laminate. 2 The sheet was irradiated with light from an LED under the conditions of 1000 kJ / s, 1000 kJ / s, and 640 seconds of irradiation time. The peak wavelength of this light was 340 nm. The light irradiation was carried out at room temperature (23°C). As a result, the coating layer was photocured, and a pressure-sensitive adhesive sheet (thickness: 20 μm) of Example 1 sandwiched between the base sheet and release liner L1 was obtained. The illuminance of the light was measured using an illuminance meter (UD-T3040T2, manufactured by Topcon Technohouse Corporation).

[0141] (Examples 2 to 13 and Comparative Examples 1 to 3) Pressure-sensitive adhesive sheets of Examples 2 to 13 and Comparative Examples 1 to 3 sandwiched between a base sheet and a release liner L1 were obtained in the same manner as in Example 1, except that the photocurable composition, light source, and light irradiation conditions used were changed as shown in Table 4. In Examples 10 to 13, an LED with a peak wavelength of 330 nm was used as the light source. In Comparative Examples 1 to 3, a black light source (B / L) was used as the light source.

[0142] [Remaining Amount of Photopolymerization Initiator] The compositions of the pressure-sensitive adhesive sheets produced in Examples 1 to 13 and Comparative Examples 1 to 3 were analyzed, and the remaining amount (content) of the photopolymerization initiator was calculated based on the results obtained. The composition analysis was performed using liquid chromatography (LC) under the following conditions.・Apparatus used: 1290 Infinity II (Agilent Technologies) ・Column: Acquity UPLC BEH C18 (Waters, 2.1 mmφ×100 mm, 1.7 μm) ・Eluent composition: Gradient conditions of ultrapure water / acetonitrile ・Column temperature: 40°C ・Column flow rate: 0.2 mL / min ・Injection volume: 2 μL ・Detector: Photodiode array detector (PDA) ・Measurement wavelength: 190 to 400 nm ・Extraction wavelength: Omnirad 184 = 246 nm, Omnirad 651 = 253 nm, Omnirad 819 = 296 nm, Omnirad 127 = 262 nm, Omnirad 2959 = 278 nm ・Sample preparation method: Approximately 0.5 g of sample (adhesive sheet) was weighed out, 2 mL of chloroform was added, and the mixture was shaken overnight. After adding 8 mL of methanol to the resulting solution, the supernatant was filtered through a 0.45 μm membrane filter, and the resulting filtrate was injected into an LC for analysis.

[0143] [Polymerization Rate of Monomer Group] For the pressure-sensitive adhesive sheets produced in Examples 1 to 13 and Comparative Examples 1 to 3, the polymerization rate of the monomer group was determined by the following method. First, the base sheet and release liner were peeled off from the pressure-sensitive adhesive sheet, and the weight W0 of the pressure-sensitive adhesive sheet (weight before drying) was measured. Next, this pressure-sensitive adhesive sheet was dried by heating at 130°C for 2 hours, and then cooled at room temperature (23°C) for approximately 20 minutes, after which the weight W1 of the pressure-sensitive adhesive sheet (weight after drying) was measured. Based on the weight W0 (g) and weight W1 (g), the polymerization rate of the monomer group was calculated using the following formula: Polymerization rate (%) = W1 / W0 × 100

[0144] [Number-average molecular weight (Mn) and weight-average molecular weight (Mw) of polymer] First, a sample was prepared having the same composition as the photocurable composition used in Examples 1 to 13 and Comparative Examples 1 to 3, except that it did not contain a crosslinking agent. The sample was irradiated with light under the conditions of the corresponding Example and Comparative Example. As a result, the monomer groups contained in the sample were polymerized to form a polymer. The number-average molecular weight (Mn) and weight-average molecular weight (Mw) of this polymer were measured.

[0145] The Mn and Mw were measured by gel permeation chromatography (GPC) using the following measuring equipment and conditions. The measuring equipment and conditions were different for the NVP-containing composition and the NVP-free composition.

[0146] (NVP-free composition) Analytical equipment: HLC-8120GPC manufactured by Tosoh Corporation Column: G7000H manufactured by Tosoh Corporation XL +GMH XL +GMH XL Column size: 7.8 mm diameter x 30 cm, total 90 cm Column temperature: 40°C Flow rate: 0.8 mL / min Injection volume: 100 μL Eluent: tetrahydrofuran Detector: differential refractometer (RI) Standard sample: polystyrene

[0147] (NVP-containing composition) Analytical equipment: Agilent 1200, manufactured by Agilent Technologies Column: TSKgel SuperAWM-H + superAW4000 + superAW2500, manufactured by Tosoh Corporation Column size: 6.0 mmφ x 15 cm each, total 45 cm Column temperature: 40°C Flow rate: 0.4 mL / min Injection volume: 40 μL Eluent: N,N-dimethylformamide (DMF) Detector: differential refractometer (RI) Standard sample: polystyrene

[0148]

[0149] As can be seen from Table 4, the photocurable composition (C2) and the illuminance of the light irradiated to the coating layer (4 mW / cm 2 When Example 2 and Comparative Example 2, which have the same thickness, are compared, the pressure-sensitive adhesive sheet of Example 2, which was produced by irradiating light using an LED under conditions of a peak wavelength of 325 nm to 350 nm, had a smaller amount of residual photopolymerization initiator than Comparative Example 2. Similarly, the pressure-sensitive adhesive sheets of Examples 1 and 3 to 13 also had a smaller amount of residual photopolymerization initiator. Furthermore, the pressure-sensitive adhesive sheets of Examples 1 to 13 had sufficiently high polymerization rates of the monomer groups. From this, it can be said that the manufacturing method of this embodiment is suitable for efficiently producing pressure-sensitive adhesive sheets.

[0150] (Examples 14 to 16 and Comparative Examples 4 to 6) Pressure-sensitive adhesive sheets of Examples 14 to 16 and Comparative Examples 4 to 6 sandwiched between a base sheet and a release liner L1 were obtained in the same manner as in Example 1, except that the photocurable composition, light source, and light irradiation conditions used were changed as shown in Table 5. In Comparative Examples 4 to 6, an LED emitting light with a peak wavelength of 365 nm was used as the light source.

[0151] [Residual Amount of Photopolymerization Initiator, Polymerization Rate of Monomer Group] For the pressure-sensitive adhesive sheets produced in Examples 14 to 16 and Comparative Examples 4 to 6, the residual amount of photopolymerization initiator and the polymerization rate of the monomer group were calculated using the method described above.

[0152] [Number-average molecular weight (Mn) and weight-average molecular weight (Mw) of polymer] Samples having the same composition as the photocurable compositions used in Examples 14 to 16 and Comparative Examples 4 to 6, except that they did not contain a crosslinking agent, were prepared, and the number-average molecular weight (Mn) and weight-average molecular weight (Mw) of the polymer were measured by the method described above.

[0153]

[0154] As can be seen from Table 5, the photocurable composition (C11) and the illuminance of the light irradiated to the coating layer (14 mW / cm 2 When Example 16 and Comparative Example 6, which have the same composition, are compared, the pressure-sensitive adhesive sheet of Example 16, which was produced by irradiating light using an LED at a peak wavelength of 325 nm to 350 nm, had a smaller amount of residual photopolymerization initiator and a higher polymerization rate of the monomer group than Comparative Example 6. Similarly, the pressure-sensitive adhesive sheets of Examples 14 and 15 also had a smaller amount of residual photopolymerization initiator and a higher polymerization rate of the monomer group. From this, it can be said that the manufacturing method of this embodiment is suitable for efficiently producing pressure-sensitive adhesive sheets.

[0155] The pressure-sensitive adhesive sheet produced by the production method of the present invention can be used, for example, in optical laminates and image display devices.

Claims

1. A method for producing a pressure-sensitive adhesive sheet, comprising the step of irradiating a coating layer containing a photocurable composition with light from a light-emitting diode to form a pressure-sensitive adhesive sheet, wherein the peak wavelength of the light irradiated to the coating layer is 325 nm to 350 nm.

2. The manufacturing method according to claim 1, wherein the peak wavelength is 340±10 nm.

3. The illuminance of the light irradiated to the coating layer is 2.0 to 30 mW / cm 2 The method according to claim 1 , 4. The method according to claim 1, wherein the light is irradiated onto a laminate comprising a base sheet, the coating layer, and a release liner in this order.

5. The method according to claim 1, wherein the coating layer is irradiated with the light for a period of 10 to 1,000 seconds.

6. The method according to claim 1, wherein the temperature of the coating layer is maintained at 10°C to 30°C while the coating layer is irradiated with the light.

7. The manufacturing method according to claim 1, wherein the coating layer is irradiated with the light in an atmosphere having an oxygen concentration of 500 vol ppm or less.

8. The method according to claim 1, wherein the photocurable composition comprises a monomer group including a (meth)acrylic monomer and / or a partial polymer of the monomer group.

9. The method according to claim 8, wherein the polymerization rate of the monomer group in the pressure-sensitive adhesive sheet is 80% or more.

10. The method according to claim 8, wherein the photocurable composition contains a photopolymerization initiator, and the amount of the photopolymerization initiator is 1.0 part by weight or less per 100 parts by weight of the total of the monomer group and the partially polymerized product.

11. The manufacturing method according to claim 10, wherein the content of the photopolymerization initiator in the adhesive sheet is 500 wtppm or less.

12. The method according to claim 1, wherein the photocurable composition contains a solvent in an amount of 5% by weight or less.

13. A method for producing an optical film with an adhesive sheet, comprising: arranging an optical film on an exposed surface of an adhesive sheet formed by the manufacturing method according to any one of claims 1 to 12 to form an optical film with an adhesive sheet.

14. The method according to claim 13, wherein the optical film comprises at least one film selected from the group consisting of a polarizing film and a retardation film.

15. A method for producing an image display device, comprising bonding an optical film with a pressure-sensitive adhesive sheet formed by the method according to claim 13 to an image display panel to form an image display device.

Citation Information

Patent Citations

  • Method for producing tacky-adhesive sheet having ultraviolet-curable acrylic tacky adhesive layer

    JP2014111715A

  • Method for manufacturing a tacky sheet possessing an ultraviolet-curable acrylic tackifier layer

    JP2014201608A

  • Polarization film with adhesive layer on both sides, and image display device

    JP2021140160A

  • Polarizing film with adhesive layer and image display device

    JP2023021976A

  • Optical laminate and image display device

    JP2024014849A

Cited By

  • Photocurable adhesive composition, adhesive, member with adhesive, method for producing adhesive, cured body, member, and method for producing cured body

    WO2026116071A1