Multilayer polyimide film and metal-clad laminate sheet
The use of a multilayer polyimide film with specific benzophenone and biphenyl skeleton residues in the non-thermoplastic layer and a metal-clad laminate structure addresses the issue of film strength loss during desmear treatment, enhancing the stability and integrity of flexible printed wiring boards.
Patent Information
- Application Number
- PCT/JP2024/009931
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-14
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional methods for producing multilayer polyimide films used in flexible printed wiring boards face challenges in maintaining film strength during desmear treatment, which can lead to cracks and tears, especially with the transition to roll-to-roll processing that increases thermal and mechanical loads.
A multilayer polyimide film with a non-thermoplastic polyimide layer containing a tetracarboxylic dianhydride residue with a benzophenone skeleton and a diamine residue with a biphenyl skeleton, where the content of these residues is optimized to promote molecular chain entanglement and maintain high film strength, is used, along with a metal-clad laminate structure.
The solution effectively suppresses the decrease in film strength due to desmear treatment, ensuring high tensile modulus and strain retention, and reduces the occurrence of defects like cracks and tears, even under continuous roll-to-roll processing conditions.
Smart Images

Figure JP2024009931_03102024_PF_FP_ABST
Abstract
Description
Multi-layer polyimide film and metal-clad laminate
[0001] The present invention relates to a multilayer polyimide film and a metal-clad laminate.
[0002] In recent years, demand for flexible printed circuit boards (hereinafter sometimes referred to as "FPCs") has been growing in line with the expansion of demand for electronic products, particularly smartphones, tablet PCs, and notebook computers. In particular, FPCs made from multilayer polyimide films containing a thermoplastic polyimide layer as an adhesive layer are expected to enjoy further growth in demand due to their excellent heat resistance and flexibility. Furthermore, in recent years, electronic devices have become lighter, smaller, and thinner, and the demand for finer FPC wiring remains strong.
[0003] When fabricating double-sided and multilayer FPCs, metal-clad laminates, consisting of a polyimide film substrate with metal foils such as copper foils bonded to both sides, are typically used. FPC manufacturing begins with the process of drilling holes (hereinafter sometimes referred to as "vias") for interlayer electrical connection. Plating the inner walls of the vias provides electrical connection between both sides of the wiring board. Via formation processes include the through-hole method, in which through-holes are drilled using a drill or laser through the metal foil and insulating layer (polyimide layer) on both sides, and the blind via method, in which the metal foil and insulating layer on one side are cut using a laser or other method, leaving the metal foil on the other side. The blind via method is frequently used, particularly for micro-FPCs, to efficiently utilize the available area.
[0004] Conventionally, in such a via formation process, a wet desmearing process (hereinafter sometimes simply referred to as "desmearing") is performed in which the laminate is treated with an alkaline potassium permanganate aqueous solution or the like under heating in order to clean the inside of the hole and the surface of the metal foil after drilling and to remove resin residue. Polyimide is easily hydrolyzed under alkaline conditions, so the strength of the film tends to decrease as a result of the desmearing process. If the film strength decreases, defects such as cracks and tears may occur in the polyimide film (i.e., the substrate of the FPC) after the desmearing process.
[0005] Furthermore, with the aim of improving productivity, the FPC manufacturing process is shifting from the conventional batch method (discontinuous process) to the roll-to-roll method (continuous process). While the roll-to-roll method promises cost reductions, if the processing time of one step is extended, the processing time of the entire process also increases, which tends to result in a greater thermal load on the substrate. Furthermore, since tension must be applied to the substrate to prevent wrinkles from occurring during transport, the roll-to-roll method tends to impose a greater mechanical load on the substrate than the batch method. For this reason, the roll-to-roll method is more likely to experience a decrease in film strength due to desmearing.
[0006] Conventionally, a method has been reported in which a heat treatment step is added between laser processing and desmearing to remove residual stress caused by laser processing and suppress the occurrence of cracks (e.g., Patent Document 1).Also reported is a method in which cracks are suppressed by using a polyimide laminated film in which the aggregation structure of polyimide is controlled (e.g., Patent Document 2).
[0007] JP 2012-186377 A JP 2017-177604 A
[0008] However, the techniques disclosed in Patent Documents 1 and 2 still have room for improvement in terms of suppressing a decrease in film strength due to desmearing.
[0009] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a multilayer polyimide film that can suppress a decrease in film strength due to a desmear treatment, and a metal-clad laminate using the same.
[0010] <Aspects of the Present Invention> The present invention includes the following aspects.
[0011] [1] A multilayer polyimide film having a non-thermoplastic polyimide layer and a thermoplastic polyimide layer disposed on at least one surface of the non-thermoplastic polyimide layer, wherein the non-thermoplastic polyimide contained in the non-thermoplastic polyimide layer has, as the tetracarboxylic acid dianhydride residue, a tetracarboxylic acid dianhydride residue containing a benzophenone skeleton, and has, as the diamine residue, a diamine residue containing a biphenyl skeleton, and the content of the diamine residue containing the biphenyl skeleton is 30 mol % or more and 100 mol % or less with respect to all diamine residues constituting the non-thermoplastic polyimide.
[0012] [2] The multilayer polyimide film according to [1], wherein the content of the tetracarboxylic dianhydride residues containing the benzophenone skeleton is 30 mol % or more and 100 mol % or less of all tetracarboxylic dianhydride residues constituting the non-thermoplastic polyimide.
[0013] [3] The multilayer polyimide film according to [1] or [2], wherein the strain retention rate after the non-thermoplastic polyimide layer is subjected to a desmear treatment under conditions of a treatment temperature of 70°C and a treatment time of 5 minutes is 80% or more.
[0014] [4] The multilayer polyimide film according to any one of [1] to [3], wherein the non-thermoplastic polyimide layer has a tensile stress at 10% strain of 220 MPa or more.
[0015] [5] The multilayer polyimide film according to any one of [1] to [4], wherein the non-thermoplastic polyimide layer has a linear expansion coefficient of 5.0 ppm / K or more and 19.0 ppm / K or less.
[0016] [6] A metal-clad laminate comprising the multilayer polyimide film according to any one of [1] to [5] above and a metal layer disposed on a main surface of at least one of the thermoplastic polyimide layers of the multilayer polyimide film.
[0017] According to the present invention, it is possible to provide a multilayer polyimide film capable of suppressing a decrease in film strength due to a desmear treatment, and a metal-clad laminate using the same.
[0018] 1 is a cross-sectional view showing an example of a multilayer polyimide film according to the present invention, and FIG. 2 is a cross-sectional view showing an example of a metal-clad laminate according to the present invention.
[0019] Preferred embodiments of the present invention will be described in detail below, but the present invention is not limited thereto. In addition, all academic and patent documents described in this specification are incorporated herein by reference.
[0020] First, the terms used in this specification will be explained. A "structural unit" refers to a repeating unit that constitutes a polymer. A "polyimide" is a polymer containing a structural unit represented by the following general formula (1) (hereinafter, sometimes referred to as "structural unit (1)").
[0021]
[0022] In general formula (1), X 1 represents a tetracarboxylic dianhydride residue (a tetravalent organic group derived from a tetracarboxylic dianhydride), and X 2 represents a diamine residue (a divalent organic group derived from a diamine).
[0023] The content of the structural unit (1) relative to all structural units constituting the polyimide is, for example, 50 mol% or more and 100 mol% or less, preferably 60 mol% or more and 100 mol% or less, more preferably 70 mol% or more and 100 mol% or less, even more preferably 80 mol% or more and 100 mol% or less, still more preferably 90 mol% or more and 100 mol% or less, and may be 100 mol%.
[0024] The "polyamic acid" is a polymer containing a structural unit represented by the following general formula (2) (hereinafter, sometimes referred to as "structural unit (2)").
[0025]
[0026] In general formula (2), A 1 represents a tetracarboxylic dianhydride residue (a tetravalent organic group derived from a tetracarboxylic dianhydride), A 2 represents a diamine residue (a divalent organic group derived from a diamine).
[0027] The content of the structural unit (2) relative to all structural units constituting the polyamic acid is, for example, 50 mol% or more and 100 mol% or less, preferably 60 mol% or more and 100 mol% or less, more preferably 70 mol% or more and 100 mol% or less, even more preferably 80 mol% or more and 100 mol% or less, still more preferably 90 mol% or more and 100 mol% or less, and may be 100 mol%.
[0028] Polyimide is an imide of polyamic acid. Therefore, when the content of the structural unit (2) relative to all structural units constituting the polyamic acid is 100 mol %, the polyimide, which is an imide of the polyamic acid, is represented by X in the general formula (1). 1 As A in general formula (2), 1 and X in general formula (1) 2 As A in general formula (2), 2 The residue is represented by:
[0029] Unless otherwise specified, the "linear expansion coefficient" refers to the linear expansion coefficient at elevated temperatures from 50° C. to 250° C. The linear expansion coefficient is measured by the same method as in the examples described below or a method equivalent thereto.
[0030] "Non-thermoplastic polyimide" refers to a polyimide that, when fixed in a film state (thickness 17.0 μm) on a metal frame and heated at a heating temperature of 450°C for 2 minutes, does not wrinkle or stretch and maintains a film shape (flat membrane shape). "Thermoplastic polyimide" refers to a polyimide that, when fixed in a film state (thickness 17.0 μm) on a metal frame and heated at a heating temperature of 450°C for 2 minutes, does not maintain a film shape. In this specification, the non-thermoplastic polyimide contained in the non-thermoplastic polyimide layer may be simply referred to as "non-thermoplastic polyimide." Furthermore, the thermoplastic polyimide contained in the thermoplastic polyimide layer may be simply referred to as "thermoplastic polyimide."
[0031] The "main surface" of a layered material (more specifically, a non-thermoplastic polyimide layer, a thermoplastic polyimide layer, a multi-layer polyimide film, etc.) refers to a surface perpendicular to the thickness direction of the layered material.
[0032] The term "benzophenone skeleton" refers to a bicyclic skeleton in which two benzene rings are bonded via a carbonyl group.
[0033] The term "biphenyl skeleton" refers to a skeleton with a two-ring structure in which two benzene rings are bonded by one single bond. Therefore, diamine residues containing a biphenyl skeleton do not include diamine residues having a fused ring, such as a 9,9-bis(4-aminophenyl)fluorene residue.
[0034] The "physical properties of the non-thermoplastic polyimide layer (tensile modulus, tensile stress at 10% strain, slope of plastic deformation region, linear expansion coefficient, strain retention, etc.)" are the physical properties of a non-thermoplastic polyimide film having the same composition and thickness as the non-thermoplastic polyimide layer. The physical properties of the non-thermoplastic polyimide film are measured by the same methods as those in the examples described below or by methods equivalent thereto.
[0035] Hereinafter, the compound name may be followed by "based" to refer to the compound and its derivatives in a comprehensive manner. Furthermore, when the compound name is followed by "based" to represent the name of a polymer, unless otherwise specified, it means that the repeating unit of the polymer is derived from the compound or its derivative. Furthermore, tetracarboxylic acid dianhydrides may be referred to as "acid dianhydrides."
[0036] Unless otherwise specified, the components and functional groups exemplified in this specification may be used alone or in combination of two or more kinds.
[0037] The drawings referred to in the following description mainly show each component in a schematic manner for ease of understanding, and the size, number, shape, etc. of each component shown may differ from the actual size, number, shape, etc. of each component due to the convenience of creating the drawings. Furthermore, for convenience of explanation, in drawings described later, the same components as those in previously described drawings may be assigned the same reference numerals, and their explanation may be omitted.
[0038] First Embodiment: Multilayer Polyimide Film The multilayer polyimide film according to the first embodiment of the present invention is a laminate including a non-thermoplastic polyimide layer and a thermoplastic polyimide layer disposed on at least one surface (one of the main surfaces) of the non-thermoplastic polyimide layer. The non-thermoplastic polyimide contained in the non-thermoplastic polyimide layer has a tetracarboxylic acid dianhydride residue containing a benzophenone skeleton as the tetracarboxylic acid dianhydride residue and a diamine residue containing a biphenyl skeleton as the diamine residue. In the first embodiment, the content of the diamine residue containing a biphenyl skeleton in the non-thermoplastic polyimide is 30 mol% or more and 100 mol% or less of all diamine residues constituting the non-thermoplastic polyimide.
[0039] Hereinafter, tetracarboxylic dianhydrides containing a benzophenone skeleton may be referred to as "BENDA," and diamines containing a biphenyl skeleton may be referred to as "BPDI."
[0040] The multilayer polyimide film according to the first embodiment can suppress a decrease in film strength due to the desmear treatment. The reason for this is presumed to be as follows.
[0041] In the multilayer polyimide film according to the first embodiment, the non-thermoplastic polyimide contains BENDA and BPDI residues, each of which contains a backbone with a high degree of free rotation, promoting entanglement of the polyimide molecular chains. On the other hand, polyimides containing BENDA residues generally exhibit low elasticity and a high coefficient of linear expansion due to the high degree of free rotation described above. However, in the first embodiment, by incorporating relatively linear BPDI residues into the molecular chain and setting the content of the BPDI residues to 30 mol% or more and 100 mol% or less relative to the total diamine residues constituting the non-thermoplastic polyimide, entanglement of the polyimide molecular chains can be promoted while ensuring the rigidity of the polyimide molecular chains. Therefore, the multilayer polyimide film according to the first embodiment can maintain high film strength (tensile modulus, tensile elongation, etc.) even after desmearing. Therefore, the multilayer polyimide film according to the first embodiment can suppress a decrease in film strength due to desmearing.
[0042] In the first embodiment, in order to further suppress a decrease in film strength due to the desmear treatment, the content of BPDI residues in the non-thermoplastic polyimide is preferably 30 mol % or more and 80 mol % or less, more preferably 30 mol % or more and 70 mol % or less, even more preferably 30 mol % or more and 60 mol % or less, and still more preferably 30 mol % or more and 50 mol % or less, based on all diamine residues constituting the non-thermoplastic polyimide.
[0043] In the first embodiment, in order to further suppress a decrease in film strength due to the desmear treatment, the content of BENDA residues in the non-thermoplastic polyimide is preferably 30 mol % or more and 100 mol % or less, more preferably 30 mol % or more and 70 mol % or less, and even more preferably 30 mol % or more and 50 mol % or less, relative to all tetracarboxylic dianhydride residues constituting the non-thermoplastic polyimide.
[0044] Hereinafter, the property of being able to suppress a decrease in film strength due to a desmear treatment may be referred to as "desmear solution resistance." The desmear solution resistance can be measured by the retention rate of the breaking strain of a film after a desmear treatment relative to the breaking strain (strain at break) of the film before the desmear treatment. Hereinafter, the retention rate of the breaking strain of a film after a desmear treatment relative to the breaking strain of the film before the desmear treatment may be referred to as "strain retention." To obtain a multilayer polyimide film having excellent desmear solution resistance, it is preferable that the strain retention rate after a desmear treatment of a non-thermoplastic polyimide layer under conditions of a treatment temperature of 70°C and a treatment time of 5 minutes is 80% or more. When a method of performing a swelling step, a roughening step, and a neutralization step described below in this order is adopted as the desmear treatment method, the "treatment temperature" and "treatment time" of the desmear treatment refer to the "treatment temperature" and "treatment time" of the roughening step, respectively.
[0045] In order to suppress deformation of the film during the manufacturing process of the metal-clad laminate, the tensile stress of the non-thermoplastic polyimide layer at 10% strain is preferably 220 MPa or more, more preferably 240 MPa or more. Furthermore, in order to reduce residual strain during the formation of the metal-clad laminate, the tensile stress of the non-thermoplastic polyimide layer at 10% strain is preferably 320 MPa or less, more preferably 310 MPa or less. Hereinafter, the tensile stress at 10% strain may be referred to as "10% strain stress." The 10% strain stress can be adjusted, for example, by changing the content of residues derived from monomers having a rigid structure (more specifically, BPDI residues, etc.).
[0046] The non-thermoplastic polyimide layer preferably has a slope of 2.0 or more in the plastic deformation region in the stress-strain curve. When the non-thermoplastic polyimide layer is resistant to plastic deformation and has high yield strength, it exhibits high resistance to tearing in an alkaline environment. The plastic deformation region refers to the strain region after the yield point in the stress-strain curve in a tensile test of a polyimide film. The property of being "resistant to plastic deformation" means that stress increases significantly in the plastic deformation region, or that the stress required for plastic deformation is large. The property of being "resistant to plastic deformation" is indicated, for example, by the slope of the plastic deformation region. The slope of the plastic deformation region is, for example, the slope of the s-s curve in the plastic deformation region of a graph in which the vertical axis is "stress (unit: MPa)" and the horizontal axis is "strain (unit: mm)" for the results of measuring tensile properties according to ASTM D882. The slope of the s-s curve in the plastic deformation region can be calculated using the following formula. In the following formula, stress1 is the stress at 10% strain, stress2 is the breaking stress, strain1 is the 10% strain, and strain2 is the breaking strain.
[0047] Slope of the s-s curve in the plastic deformation region = (stress2 - stress1) / (strain2 - strain1)
[0048] The slope of the plastic deformation region of the non-thermoplastic polyimide layer is preferably 2.0 or more, more preferably 2.2 or more. When the slope of the plastic deformation region is 2.0 or more, an aggregate structure with a high degree of packing of polymer chains is formed, and the occurrence of cracks can be suppressed even in continuous FPC processing steps. A higher slope of the plastic deformation region is better, but in order to suppress the occurrence of springback, etc., the slope of the plastic deformation region is preferably 4.5 or less, more preferably 4.0 or less.
[0049] The linear expansion coefficient of the non-thermoplastic polyimide layer is preferably 5.0 ppm / K or more and 19.0 ppm / K or less, more preferably 6.0 ppm / K or more and 15.0 ppm / K or less, and even more preferably 7.0 ppm / K or more and 12.0 ppm / K or less. If the linear expansion coefficient of the non-thermoplastic polyimide layer is 5.0 ppm / K or more and 19.0 ppm / K or less, the linear expansion coefficient of the multilayer polyimide film can be adjusted, for example, to 14.0 ppm / K or more and 22.0 ppm / K or less, which is close to that of copper foil, and preferably to 16.0 ppm / K or more and 20.0 ppm / K or less, which is even closer to that of copper foil. This reduces the difference in thermal expansion between the copper foil and the film when the copper foil and the multilayer polyimide film are bonded together at high temperatures. As a result, dimensional changes in the resulting copper-clad laminate (FCCL) can be suppressed. The linear expansion coefficient can be adjusted, for example, by changing the content of residues derived from monomers having a rigid structure (more specifically, BPDI residues, etc.) and the content of residues derived from monomers having a bent structure (more specifically, BENDA residues, etc.).
[0050] [Configuration of Multilayer Polyimide Film] Next, the configuration of the multilayer polyimide film according to the first embodiment will be described with reference to the drawings.
[0051] FIG. 1 is a cross-sectional view showing an example of a multilayer polyimide film according to the first embodiment. As shown in FIG. 1, the multilayer polyimide film 10 includes a non-thermoplastic polyimide layer 11 and a thermoplastic polyimide layer 12 disposed on at least one side of the non-thermoplastic polyimide layer 11. The non-thermoplastic polyimide contained in the non-thermoplastic polyimide layer 11 has a BENDA residue as the tetracarboxylic dianhydride residue and a BPDI residue as the diamine residue. In the multilayer polyimide film 10, the content of the BPDI residue in the non-thermoplastic polyimide is 30 mol % or more and 100 mol % or less relative to the total diamine residues constituting the non-thermoplastic polyimide.
[0052] In the multilayer polyimide film 10 shown in FIG. 1 , the thermoplastic polyimide layer 12 is provided on only one side of the non-thermoplastic polyimide layer 11. However, the thermoplastic polyimide layer 12 may be provided on both sides (both main surfaces) of the non-thermoplastic polyimide layer 11. When the thermoplastic polyimide layer 12 is provided on both sides of the non-thermoplastic polyimide layer 11, the two thermoplastic polyimide layers 12 may contain the same type of thermoplastic polyimide or different types of thermoplastic polyimides. The thicknesses of the two thermoplastic polyimide layers 12 may be the same or different. In the present invention, two or more layers of both the non-thermoplastic polyimide layer 11 and the thermoplastic polyimide layer 12 may be provided. In the following description, the term "multilayer polyimide film 10" includes a film in which the thermoplastic polyimide layer 12 is provided on only one side of the non-thermoplastic polyimide layer 11, a film in which the thermoplastic polyimide layer 12 is provided on both sides of the non-thermoplastic polyimide layer 11, and a film in which two or more layers of both the non-thermoplastic polyimide layer 11 and the thermoplastic polyimide layer 12 are provided.
[0053] The thickness of the multilayer polyimide film 10 (total thickness of each layer) is, for example, 6 μm or more and 60 μm or less. The thinner the multilayer polyimide film 10, the easier it is to reduce the weight of the resulting FPC and improve the foldability of the resulting FPC. In order to more easily reduce the weight of the FPC while maintaining mechanical strength and to further improve the foldability of the FPC, the thickness of the multilayer polyimide film 10 is preferably 7 μm or more and 30 μm or less, and more preferably 10 μm or more and 25 μm or less. The thickness of the multilayer polyimide film 10 can be measured using a laser hologram.
[0054] In order to easily achieve a thin FPC while ensuring adhesion between the main surface 12a of the thermoplastic polyimide layer 12 and the metal foil, the thickness of the thermoplastic polyimide layer 12 (when two or more thermoplastic polyimide layers 12 are provided, the thickness of each thermoplastic polyimide layer 12) is preferably 1 μm or more and 15 μm or less. Furthermore, in order to easily adjust the linear expansion coefficient of the multilayer polyimide film 10, the thickness ratio of the non-thermoplastic polyimide layer 11 to the thermoplastic polyimide layer 12 (thickness of the non-thermoplastic polyimide layer 11 / thickness of the thermoplastic polyimide layer 12) is preferably 55 / 45 or more and 95 / 5 or less. When at least one of the non-thermoplastic polyimide layer 11 and the thermoplastic polyimide layer 12 is provided in multiple layers, the thickness used to calculate the thickness ratio is the total thickness. Even if the number of thermoplastic polyimide layers 12 is increased, it is preferable that the total thickness of the thermoplastic polyimide layers 12 does not exceed the total thickness of the non-thermoplastic polyimide layers 11.
[0055] In order to suppress warping of the multilayer polyimide film 10, it is preferable that a thermoplastic polyimide layer 12 be provided on both sides of the non-thermoplastic polyimide layer 11, and it is more preferable that a thermoplastic polyimide layer 12 containing the same type of thermoplastic polyimide be provided on both sides of the non-thermoplastic polyimide layer 11. When a thermoplastic polyimide layer 12 is provided on both sides of the non-thermoplastic polyimide layer 11, it is preferable that the thicknesses of the two thermoplastic polyimide layers 12 be the same in order to suppress warping of the multilayer polyimide film 10. Even if the thicknesses of the two thermoplastic polyimide layers 12 are different from each other, warping of the multilayer polyimide film 10 can be suppressed as long as the thickness of the other thermoplastic polyimide layer 12 is in the range of 40% or more and less than 100% of the thickness of the thicker thermoplastic polyimide layer 12.
[0056] [Elements of Multilayer Polyimide Film] Next, the elements (constituent elements) of the multilayer polyimide film according to the first embodiment will be described in detail.
[0057] (Non-thermoplastic Polyimide Layer) The non-thermoplastic polyimide contained in the non-thermoplastic polyimide layer has a BPDI residue as the diamine residue. Examples of diamines (monomers) for forming the BPDI residue include 4,4'-diamino-2,2'-dimethylbiphenyl (hereinafter sometimes referred to as "m-TB"), 4,4'-diaminobiphenyl, 4,4'-diamino-3,3'-dimethylbiphenyl, 4,4'-diamino-2,2'-dimethoxybiphenyl, 4,4'-diamino-3,3'-dimethoxybiphenyl, 3,3',5,5'-tetramethylbenzidine, and 4,4'-bis(4-aminophenoxy)biphenyl. In this embodiment, one or more diamines can be used as the diamine for forming the BPDI residue. In order to further suppress a decrease in film strength due to the desmear treatment, m-TB is preferred as the diamine (monomer) for forming the BPDI residue. In other words, the BPDI residue is preferably an m-TB residue.
[0058] The non-thermoplastic polyimide may have a diamine residue other than the BPDI residue (another diamine residue) as the diamine residue. A highly heat-resistant aromatic diamine is preferable as the diamine (monomer) for forming the other diamine residue. Specific examples of the diamine for forming the other diamine residue include p-phenylenediamine (hereinafter sometimes referred to as "PDA"), 4,4'-diaminodiphenyl ether (hereinafter sometimes referred to as "ODA"), 2,2-bis[4-(4-aminophenoxy)phenyl]propane (hereinafter sometimes referred to as "BAPP"), 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-diaminodiphenylpropane, 4,4'-diaminodiphenylmethane, and 4,4'-diaminodiphenylsulfonyl. Examples of the diaminodiphenyl ether include 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 1,5-diaminonaphthalene, 4,4'-diaminodiphenyldiethylsilane, 4,4'-diaminodiphenylsilane, 4,4'-diaminodiphenylethylphosphine oxide, 4,4'-diaminodiphenyl N-methylamine, 4,4'-diaminodiphenyl N-phenylamine, 1,3-diaminobenzene, 1,2-diaminobenzene, and derivatives thereof.
[0059] As the other diamine residue, a combination of one or more diamine residues having a flexible structure selected from the group consisting of an ODA residue, a BAPP residue, a 1,3-diaminobenzene residue, and a 1,3-bis(4-aminophenoxy)benzene residue and a PDA residue having a rigid structure is preferred, and a combination of an ODA residue and a PDA residue is more preferred.
[0060] The content of other diamine residues is 0 mol% or more and 70 mol% or less relative to all diamine residues constituting the non-thermoplastic polyimide. From the viewpoint of ensuring high heat resistance, the content of diamine residues having a rigid structure among the other diamine residues is preferably 10 mol% or more and 50 mol% or less, more preferably 15 mol% or more and 40 mol% or less, and even more preferably 15 mol% or more and 35 mol% or less, relative to all diamine residues constituting the non-thermoplastic polyimide. Furthermore, in order to adjust the linear expansion coefficient of the multilayer polyimide film within an appropriate range, the content of diamine residues having a flexible structure among the other diamine residues is preferably 20 mol% or more and 60 mol% or less, more preferably 25 mol% or more and 55 mol% or less, and even more preferably 30 mol% or more and 50 mol% or less, relative to all diamine residues constituting the non-thermoplastic polyimide.
[0061] The non-thermoplastic polyimide contained in the non-thermoplastic polyimide layer has a BENDA residue as the acid dianhydride residue. Examples of the acid dianhydride (monomer) for forming the BENDA residue include 3,3',4,4'-benzophenonetetracarboxylic dianhydride (hereinafter sometimes referred to as "BTDA"), 2,2',3,3'-benzophenonetetracarboxylic dianhydride, and 2,3,3',4'-benzophenonetetracarboxylic dianhydride. In this embodiment, one or more acid dianhydrides can be used as the acid dianhydride for forming the BENDA residue. In order to further suppress a decrease in film strength due to the desmear treatment, BTDA is preferred as the acid dianhydride (monomer) for forming the BENDA residue. In other words, the BTDA residue is preferred as the BENDA residue.
[0062] The non-thermoplastic polyimide may have an acid dianhydride residue other than the BENDA residue (another acid dianhydride residue) as the acid dianhydride residue. Examples of the acid dianhydride (monomer) for forming the other acid dianhydride residue include pyromellitic dianhydride (hereinafter sometimes referred to as "PMDA"), 3,3',4,4'-biphenyltetracarboxylic dianhydride (hereinafter sometimes referred to as "BPDA"), 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, and 4,4'-oxydiphthalic anhydride (hereinafter sometimes referred to as "ODPA"). , 3,4'-oxydiphthalic anhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, p-phenylene bis(trimellitic acid monoester acid anhydride), ethylene bis(trimellitic acid monoester acid anhydride), bisphenol A bis(trimellitic acid monoester acid anhydride), and derivatives thereof.
[0063] From the viewpoint of ensuring high heat resistance and low thermal expansion, the other acid dianhydride residues are preferably one or more selected from the group consisting of PMDA residues, BPDA residues, and ODPA residues, more preferably one or more selected from the group consisting of PMDA residues and BPDA residues, and even more preferably PMDA residues. From the viewpoint of ensuring high heat resistance and low thermal expansion, the content of the other acid dianhydride residues is preferably 70 mol% or less, more preferably 10 mol% or more and 70 mol% or less, even more preferably 30 mol% or more and 70 mol% or less, and even more preferably 50 mol% or more and 70 mol% or less, based on the total acid dianhydride residues constituting the non-thermoplastic polyimide.
[0064] In order to maintain a good surface appearance of the metal-clad laminate while suppressing the occurrence of cracks and tears in the film during the FPC manufacturing process, it is preferable that the non-thermoplastic polyimide has a segment whose repeating unit is a structural unit represented by the following chemical formula (3). In this specification, the term "segment" refers to a polymer chain formed from the same repeating unit that constitutes a block copolymer. In this specification, the term "block copolymer" includes all aspects of a pure block copolymer, a random block copolymer, and a copolymer having a tapered block structure.
[0065]
[0066] A segment having a structural unit represented by chemical formula (3) as a repeating unit (hereinafter, sometimes referred to as a "specific segment") can be formed, for example, by sequence polymerization, which will be described later.
[0067] The non-thermoplastic polyimide layer may contain components (additives) other than the non-thermoplastic polyimide. Examples of additives that can be used include dyes, surfactants, leveling agents, plasticizers, silicones, fillers, and sensitizers. The content of the non-thermoplastic polyimide in the non-thermoplastic polyimide layer is, for example, 70% by weight or more, preferably 80% by weight or more, more preferably 90% by weight or more, and may be 100% by weight, based on the total weight of the non-thermoplastic polyimide layer.
[0068] (Thermoplastic Polyimide Layer) The thermoplastic polyimide contained in the thermoplastic polyimide layer has an acid dianhydride residue and a diamine residue. The acid dianhydride (monomer) for forming the acid dianhydride residue in the thermoplastic polyimide can be the same compound as the acid dianhydride (monomer) for forming the acid dianhydride residue in the non-thermoplastic polyimide described above. The acid dianhydride residue in the thermoplastic polyimide and the acid dianhydride residue in the non-thermoplastic polyimide can be the same or different.
[0069] In order to ensure thermoplasticity, the diamine residue contained in the thermoplastic polyimide is preferably a diamine residue having a bent structure. In order to more easily ensure thermoplasticity, the content of the diamine residue having a bent structure is preferably 50 mol% or more, more preferably 70 mol% or more, and even more preferably 80 mol% or more, relative to the total diamine residues constituting the thermoplastic polyimide, and may even be 100 mol%. Examples of diamines (monomers) for forming the diamine residue having a bent structure include 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)biphenyl, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, and BAPP. In order to more easily ensure thermoplasticity, the diamine residue contained in the thermoplastic polyimide is preferably a BAPP residue.
[0070] In order to obtain a thermoplastic polyimide layer having excellent adhesion to a metal foil, the thermoplastic polyimide preferably contains one or more selected from the group consisting of BPDA residues and PMDA residues, and a BAPP residue. Furthermore, in order to further suppress a decrease in film strength due to a desmear treatment, the total content of BPDA residues and PMDA residues is preferably 85 mol% to 100 mol%, more preferably more than 85 mol% to 100 mol%, even more preferably 90 mol% to 100 mol%, even more preferably 95 mol% to 100 mol%, and particularly preferably 100 mol%, based on the total acid dianhydride residues constituting the thermoplastic polyimide.
[0071] The thermoplastic polyimide layer may contain components (additives) other than the thermoplastic polyimide. Examples of the additives that can be used include dyes, surfactants, leveling agents, plasticizers, silicones, fillers, and sensitizers. The content of the thermoplastic polyimide in the thermoplastic polyimide layer is, for example, 70% by weight or more, preferably 80% by weight or more, more preferably 90% by weight or more, and may be 100% by weight, based on the total weight of the thermoplastic polyimide layer.
[0072] [Preferred Aspects of the First Embodiment] In order to ensure high heat resistance and low thermal expansion while further suppressing a decrease in film strength due to a desmear treatment, the multilayer polyimide film according to the first embodiment preferably satisfies the following condition 1, more preferably satisfies the following condition 2, and even more preferably satisfies the following condition 3. Furthermore, in order to obtain a multilayer polyimide film that can effectively suppress a decrease in film strength due to a desmear treatment while adjusting the linear expansion coefficient of the film within an appropriate range and can ensure high heat resistance, the multilayer polyimide film according to the first embodiment preferably satisfies the following condition 4. Condition 1: The content of BPDI residues in the non-thermoplastic polyimide is 30 mol % or more and 70 mol % or less relative to all diamine residues constituting the non-thermoplastic polyimide, and the content of BENDA residues in the non-thermoplastic polyimide is 30 mol % or more and 70 mol % or less relative to all tetracarboxylic dianhydride residues constituting the non-thermoplastic polyimide. Condition 2: The above condition 1 is satisfied, and the non-thermoplastic polyimide further has a PDA residue as a diamine residue. Condition 3: The above condition 2 is satisfied, and the non-thermoplastic polyimide further has a PMDA residue as an acid dianhydride residue.Condition 4: The above condition 3 is satisfied, and the non-thermoplastic polyimide further has an ODA residue as a diamine residue.
[0073] <Second embodiment: metal-clad laminate> Next, a metal-clad laminate according to a second embodiment of the present invention will be described. The metal-clad laminate according to the second embodiment of the present invention is a metal-clad laminate obtained using the multilayer polyimide film according to the first embodiment of the present invention described above. In the following description, the description of the same content as in the first embodiment may be omitted.
[0074] The metal-clad laminate according to the second embodiment has the multilayer polyimide film according to the first embodiment and a metal layer disposed on the main surface of at least one of the thermoplastic polyimide layers of the multilayer polyimide film. According to the second embodiment, since the multilayer polyimide film according to the first embodiment is provided, defects (cracks, tears, etc.) in the substrate (multilayer polyimide film) can be suppressed during the FPC manufacturing process. Hereinafter, an example of the metal-clad laminate according to the second embodiment will be described with reference to FIG. 2. FIG. 2 is a cross-sectional view showing an example of the metal-clad laminate according to the second embodiment.
[0075] As shown in FIG. 2, the metal-clad laminate 20 has a multilayer polyimide film 10 and a metal layer 13 disposed on a main surface 12 a of at least one thermoplastic polyimide layer 12 of the multilayer polyimide film 10 .
[0076] A metal foil can be used as the metal layer 13. The metal foil is not particularly limited, and any metal foil can be used. For example, metal foils made of copper, stainless steel, nickel, aluminum, alloys of these metals, etc. are preferably used. In addition, copper foils such as rolled copper foils and electrolytic copper foils are often used in general metal-clad laminates, and copper foils are also preferably used in the second embodiment.
[0077] Furthermore, the metal foil can be used after being subjected to a surface treatment or the like to adjust the surface roughness, etc., depending on the purpose. Furthermore, an anti-rust layer, a heat-resistant layer, an adhesive layer, etc., may be formed on the surface of the metal foil. The thickness of the metal layer 13 is not particularly limited, and it is sufficient as long as it can exhibit sufficient functionality depending on the application. In order to easily achieve a thinner FPC while suppressing the occurrence of wrinkles when bonding with the multilayer polyimide film 10, the thickness of the metal layer 13 is preferably 5 μm or more and 50 μm or less.
[0078] When manufacturing a metal-clad laminate 20 using the multilayer polyimide film 10, a metal foil to become the metal layer 13 is laminated to at least one surface of the multilayer polyimide film 10 (for example, the main surface 12a of the thermoplastic polyimide layer 12 in the case of FIG. 2). The method for laminating the metal foil to the main surface 12a of the thermoplastic polyimide layer 12 is not particularly limited, and various known methods can be used. For example, a continuous processing method using a hot roll laminating device having one or more pairs of metal rolls or a double belt press (DBP) can be used. The specific configuration of the means for performing hot roll lamination is not particularly limited, but it is preferable to place a protective material between the pressure surface and the metal foil to improve the appearance of the resulting metal-clad laminate 20.
[0079] When the thermoplastic polyimide layer 12 is provided on both sides of the non-thermoplastic polyimide layer 11, a double-sided metal-clad laminate (not shown) can be obtained by laminating metal foil to both sides of the multilayer polyimide film 10.
[0080] When an FPC is manufactured using the metal-clad laminate 20, the yield rate of the FPC can be increased even when a roll-to-roll system is employed. In other words, even when desmearing is performed using the roll-to-roll system, a decrease in the strength of the multilayer polyimide film 10 in the metal-clad laminate 20 is suppressed, and therefore, the occurrence of defects in the substrate (multilayer polyimide film 10) can be suppressed in the FPC manufacturing process. As the desmearing method, a known method can be used, and examples thereof include a wet desmearing method including a swelling step using an alkaline aqueous solution or a solution containing an organic solvent, a roughening step using an alkaline aqueous solution containing sodium permanganate, potassium permanganate, or the like, and a neutralization step.
[0081] <Method for Producing Multilayer Polyimide Film> Next, an example of a method for producing the multilayer polyimide film according to the first embodiment will be described.
[0082] [Method for Producing Polyamic Acid] Polyamic acid, a precursor of polyimide, can be produced (synthesized) by any known method or a combination thereof. A key feature of the polymerization method for producing polyamic acid is the order of monomer addition. Controlling the order of monomer addition allows for control of the properties of the resulting polyimide. When synthesizing polyamic acid using a diamine and a tetracarboxylic dianhydride, the desired polyamic acid (a polymer of a diamine and a tetracarboxylic dianhydride) can be obtained by adjusting the molar amount of the diamine (or, if multiple diamines are used, the molar amount of each diamine) and the molar amount of the tetracarboxylic dianhydride (or, if multiple tetracarboxylic dianhydrides are used, the molar amount of each tetracarboxylic dianhydride). The molar fraction of each residue in the polyimide formed from the polyamic acid corresponds, for example, to the molar fraction of each monomer (diamine and tetracarboxylic dianhydride) used in the synthesis of the polyamic acid. The temperature conditions for the reaction between the diamine and the tetracarboxylic dianhydride, i.e., the polyamic acid synthesis reaction, are not particularly limited, but are typically in the range of 10°C to 150°C. The reaction time for the synthesis reaction of polyamic acid is, for example, in the range of 10 minutes to 30 hours. Any method for adding monomers may be used to produce polyamic acid. Typical methods for producing polyamic acid include the following.
[0083] Examples of methods for producing polyamic acid include a polymerization method (hereinafter sometimes referred to as "polymerization method A") that involves the following steps (A-a) and (A-b): (A-a): a step of reacting an aromatic diamine with an aromatic acid dianhydride in an organic solvent with the aromatic diamine in excess to obtain a prepolymer having amino groups at both ends; (A-b): a step of adding an additional aromatic diamine having a different structure from that used in step (A-a), and then adding an aromatic acid dianhydride having a different structure from that used in step (A-a) so that the aromatic diamine and aromatic acid dianhydride are substantially equimolar in all steps, and polymerizing the resulting mixture.
[0084] Another example of a method for producing polyamic acid is a polymerization method (hereinafter sometimes referred to as "polymerization method B") that involves the following steps (Ba) and (B-b): (Ba): a step of reacting an aromatic diamine with an aromatic acid dianhydride in an organic solvent with an excess of the aromatic acid dianhydride to obtain a prepolymer having acid anhydride groups at both ends; (B-b): a step of adding an aromatic acid dianhydride having a different structure from that used in step (Ba), and then adding an aromatic diamine having a different structure from that used in step (Ba) so that the aromatic diamine and aromatic acid dianhydride are substantially equimolar in all steps, and polymerizing the resulting mixture.
[0085] A polymerization method in which the addition order is set so that a specific diamine or specific acid dianhydride selectively reacts with any or specific diamine, or any or specific acid dianhydride (for example, the above-mentioned polymerization method A or polymerization method B) is referred to herein as sequence polymerization. Among polymers obtained by sequence polymerization, a polymer having two types of segments is called a diblock copolymer, and a polymer having three types of segments is called a triblock copolymer. In contrast, a polymerization method in which the addition order of diamine and acid dianhydride is not set (a polymerization method in which monomers react with each other randomly) is referred to herein as random polymerization. A polymer obtained by random polymerization is called a random copolymer.
[0086] As a polymerization method for obtaining a polyimide that can further suppress the decrease in film strength due to the desmear treatment, sequence polymerization is preferred.
[0087] The weight-average molecular weight of the polyamic acid obtained by the above-mentioned polymerization method is preferably in the range of 10,000 to 1,000,000, more preferably in the range of 20,000 to 500,000, and even more preferably in the range of 30,000 to 200,000. If the weight-average molecular weight is 10,000 or more, it is easy to form the polyamic acid into a coating film. On the other hand, if the weight-average molecular weight is 1,000,000 or less, it exhibits sufficient solubility in solvents, so that a coating film with a smooth surface and uniform thickness can be obtained using a polyamic acid solution described below. The weight-average molecular weight used here refers to a polyethylene oxide equivalent value measured using gel permeation chromatography (GPC).
[0088] When obtaining a polyimide, a method of obtaining the polyimide from a polyamic acid solution containing a polyamic acid and an organic solvent may be employed. Examples of organic solvents that can be used in polyamic acid solutions include urea-based solvents such as tetramethylurea and N,N-dimethylethylurea; sulfoxide-based solvents such as dimethyl sulfoxide; sulfone-based solvents such as diphenyl sulfone and tetramethyl sulfone; amide-based solvents such as N,N-dimethylacetamide, N,N-dimethylformamide (hereinafter sometimes referred to as "DMF"), N,N-diethylacetamide, N-methyl-2-pyrrolidone, and hexamethylphosphoric triamide; ester-based solvents such as γ-butyrolactone; alkyl halide-based solvents such as chloroform and methylene chloride; aromatic hydrocarbon-based solvents such as benzene and toluene; phenol-based solvents such as phenol and cresol; ketone-based solvents such as cyclopentanone; and ether-based solvents such as tetrahydrofuran, 1,3-dioxolane, 1,4-dioxane, dimethyl ether, diethyl ether, diethylene glycol diethyl ether, diethylene glycol dimethyl ether, and p-cresol methyl ether. These solvents are usually used alone, but two or more of them may be used in combination as needed. When polyamic acid is obtained by the above-mentioned polymerization method, the reaction solution (the solution after the reaction) itself may be used as a polyamic acid solution for obtaining a polyimide. In this case, the organic solvent in the polyamic acid solution is the organic solvent used in the reaction in the above-mentioned polymerization method. Alternatively, the solid polyamic acid obtained by removing the solvent from the reaction solution may be dissolved in an organic solvent to prepare a polyamic acid solution.
[0089] The polyamic acid solution may contain additives such as dyes, surfactants, leveling agents, plasticizers, silicones, and sensitizers. Furthermore, a filler may be added to the polyamic acid solution to improve various film properties such as sliding properties, thermal conductivity, electrical conductivity, corona resistance, and loop stiffness. Any filler may be used, but preferred examples include fillers made of silica, titanium oxide, alumina, silicon nitride, boron nitride, calcium hydrogen phosphate, calcium phosphate, mica, and the like.
[0090] The concentration of polyamic acid in the polyamic acid solution is not particularly limited and is, for example, 5 to 35% by weight, preferably 8 to 30% by weight, based on the total amount of the polyamic acid solution. When the concentration of polyamic acid is 5 to 35% by weight, an appropriate molecular weight and solution viscosity can be obtained.
[0091] [Method for Forming a Non-Thermoplastic Polyimide Layer] The method for forming the non-thermoplastic polyimide layer is not particularly limited, and various known methods can be applied. For example, a method for forming a non-thermoplastic polyimide layer (polyimide film) through the following steps i) to iv) can be mentioned. Step i): A step of reacting an aromatic diamine with an aromatic tetracarboxylic dianhydride in an organic solvent to obtain a polyamic acid solution containing a precursor of a non-thermoplastic polyimide (hereinafter, may be referred to as a "non-thermoplastic polyamic acid solution"); Step ii): A step of applying a dope liquid containing the non-thermoplastic polyamic acid solution onto a support to form a coating film; Step iii): A step of heating the coating film on the support to form a self-supporting polyamic acid film (hereinafter, may be referred to as a "gel film"), and then peeling the gel film from the support; Step iv): A step of heating the gel film to imidize the polyamic acid in the gel film and drying it to obtain a polyimide film containing a non-thermoplastic polyimide (a polyimide film that will become the non-thermoplastic polyimide layer in the multilayer polyimide film).
[0092] In step ii), the method for applying the dope solution onto the support is not particularly limited, and a method using a conventionally known coating device such as a die coater, a comma coater (registered trademark), a reverse coater, or a knife coater can be used.
[0093] The steps from step ii) onwards are broadly divided into thermal imidization and chemical imidization. Thermal imidization is a method in which a polyamic acid solution is applied as a dope onto a support without using a dehydrating ring-closing agent or the like, and the imidization is promoted by heating. On the other hand, chemical imidization is a method in which a polyamic acid solution to which at least one of a dehydrating ring-closing agent and a catalyst has been added as an imidization accelerator is used as a dope to accelerate imidization. Either method may be used, but chemical imidization is more productive.
[0094] As the dehydration ring-closing agent, an acid anhydride typified by acetic anhydride is preferably used. As the catalyst, a tertiary amine such as an aliphatic tertiary amine, an aromatic tertiary amine, or a heterocyclic tertiary amine is preferred, and isoquinoline is more preferred.
[0095] In step ii), the support to which the dope solution is applied is preferably a glass plate, aluminum foil, an endless stainless steel belt, a stainless steel drum, etc. In step iii), heating conditions are set depending on the thickness of the film to be finally obtained and the production rate, and the film is partially imidized or dried, and then peeled off from the support to obtain a polyamic acid film (gel film).
[0096] Next, in step iv), for example, the gel film is heated while fixing the edges to avoid shrinkage during curing, thereby removing water, residual solvent, imidization accelerator, etc. from the gel film and completely imidizing the remaining polyamic acid, thereby obtaining a polyimide film containing a non-thermoplastic polyimide. The heating conditions may be appropriately set depending on the thickness of the final film to be obtained and the production speed.
[0097] [Method for Forming a Thermoplastic Polyimide Layer] The thermoplastic polyimide layer can be formed, for example, by applying a polyamic acid solution (hereinafter sometimes referred to as a "thermoplastic polyamic acid solution") containing a polyamic acid, which is a precursor of a thermoplastic polyimide, to at least one side of a polyimide film (non-thermoplastic polyimide layer) obtained using the non-thermoplastic polyamic acid solution described above, followed by heating (drying and imidization of the polyamic acid). This method can produce a multilayer polyimide film having a non-thermoplastic polyimide layer and a thermoplastic polyimide layer disposed on at least one side of the non-thermoplastic polyimide layer. Alternatively, a solution containing a thermoplastic polyimide (thermoplastic polyimide solution) can be used instead of the thermoplastic polyamic acid solution to form a coating film of the thermoplastic polyimide solution on at least one side of the non-thermoplastic polyimide layer, and the coating film can be dried to form a thermoplastic polyimide layer.
[0098] Alternatively, for example, a co-extrusion die may be used to form a laminate on a support, the laminate comprising a layer containing a polyamic acid, which is a precursor of a non-thermoplastic polyimide, and a layer containing a polyamic acid, which is a precursor of a thermoplastic polyimide, and then the resulting laminate may be heated to simultaneously form a non-thermoplastic polyimide layer and a thermoplastic polyimide layer. Alternatively, a laminate may be formed by continuous coating (continuous casting) the laminate comprising a layer containing a polyamic acid, which is a precursor of a non-thermoplastic polyimide, and a layer containing a polyamic acid, which is a precursor of a thermoplastic polyimide, and then the resulting laminate may be heated to simultaneously form a non-thermoplastic polyimide layer and a thermoplastic polyimide layer. In these methods, by using a metal foil as the support, a metal-clad laminate (a laminate of a multilayer polyimide film and a metal foil) is obtained as soon as imidization is completed. When producing a multilayer polyimide film containing three or more polyimide layers, the above-mentioned coating and heating steps may be repeated multiple times, or multiple coating films may be formed by co-extrusion or continuous coating (continuous casting) and then heated at the same time. Various surface treatments, such as corona treatment and plasma treatment, may also be performed on the outermost surface of the multilayer polyimide film.
[0099] The present invention will be specifically explained below with reference to examples, but the present invention is not limited to these examples.
[0100] <Methods for Measuring Physical Properties> First, methods for measuring physical properties of polyimide films will be described.
[0101] [Tensile modulus, stress at 10% strain, and slope of plastic deformation region] The tensile modulus of the polyimide film was measured in accordance with ASTM D882 using a precision universal testing machine ("AUTOGRAPH AGS-J" manufactured by Shimadzu Corporation). The stress at 10% strain was read from the measurement data of the tensile modulus. The slope of the plastic deformation region was calculated from the measurement data of the tensile modulus according to the above-mentioned formula. The measurement conditions for the tensile modulus are as follows: Width of sample (polyimide film): 15 mm Distance between grippers: 100 mm Tensile speed: 200 mm / min Measurement environment: Temperature 23°C and humidity 55% RH
[0102] [Coefficient of Linear Expansion (CTE)] Using a thermal analyzer ("TMA / SS6100" manufactured by Hitachi High-Tech Science Corporation), a polyimide film was heated in a nitrogen atmosphere from -10°C to 300°C at a heating rate of 10°C / min, then cooled to -10°C at a heating rate of 40°C / min, and heated again to 300°C at a heating rate of 10°C / min, and the coefficient of linear expansion was determined from the amount of strain during the second heating from 50°C to 250°C. The measurement conditions are as follows: Sample (polyimide film) size: width 3 mm, length 10 mm Load: 1 g (9.8 mN)
[0103] [Resistance to Desmear Solution] (Desmear Treatment Conditions) Table 1 shows the desmear treatment conditions for evaluating the resistance of polyimide films to desmear solutions. In Table 1, the values in the "Concentration" column indicate the concentrations in the treatment solution (aqueous solution). A water-washing step was carried out between the swelling step and the roughening step, and between the roughening step and the neutralization step. A water-washing step and a drying step were carried out after the neutralization step. The chemical solutions used in the swelling step and the roughening step were both manufactured by MacDermid Performance Solutions Japan, Inc. The chemical solution used in the neutralization step was manufactured by Rohm and Haas Electronic Materials, Inc.
[0104]
[0105] (Measurement of Breaking Strain) For the polyimide film before desmearing and the polyimide film after desmearing under the above conditions, the breaking strain (strain at break) was measured using a precision universal testing machine ("AUTOGRAPH AGS-J" manufactured by Shimadzu Corporation) under the following conditions in accordance with ASTM D882. Shape of measurement sample: No. 6 dumbbell shape Width of measurement point on measurement sample: 4 mm Distance between grippers: 25 mm Pulling speed: 25 mm / min Measurement environment: Temperature 23°C and humidity 55% RH
[0106] Next, the strain retention rate (unit: %) was calculated according to the formula "strain retention rate = 100 × breaking strain of polyimide film after desmear treatment / breaking strain of polyimide film before desmear treatment". A strain retention rate of 80% or more was judged as "A", a strain retention rate of 50% or more and less than 80% was judged as "B", and a strain retention rate of less than 50% was judged as "C". When the judgment result was A, it was evaluated that "a decrease in film strength due to the desmear treatment was suppressed". On the other hand, when the judgment result was B or C, it was evaluated that "a decrease in film strength due to the desmear treatment was not suppressed".
[0107] [Peel Strength] Electrodeposited copper foils ("3EC-M3S-HTE" manufactured by Mitsui Mining & Smelting Co., Ltd.) having a thickness of 12 μm were placed on both sides of the multilayer polyimide film, and protective films ("Apical 125NPI" manufactured by Kaneka Corporation, thickness: 125 μm) were placed on the outer surfaces of each of the electrolytic copper foils. Lamination was then performed under the conditions of a lamination temperature of 360° C., a lamination pressure of 307.7 N / cm, and a lamination speed of 1.0 m / min to obtain a flexible copper-clad laminate (FCCL).
[0108] Then, in accordance with JIS C6471-1995, the average value of the peel strength when 30 mm of the electrodeposited copper foil (width: 1 mm) on one side of the FCCL was peeled off using a tensile tester (Strograph VES1D manufactured by Toyo Seiki Seisaku-sho, Ltd.) under conditions of a temperature of 23°C and a humidity of 55% RH, a pulling rate of 50 mm / min, and a peel angle of 90° was defined as the peel strength. In all of Examples 1 to 6 and Comparative Examples 1 to 5 described below, the peel strength was 12 N / cm or more.
[0109] <Preparation of Polyamic Acid Solutions> Below, we will explain how to prepare solutions P1 to P11, which are non-thermoplastic polyamic acid solutions, and solution P12, which is a thermoplastic polyamic acid solution. All of solutions P1 to P12 were prepared in a nitrogen atmosphere at 20°C. In the following, compounds and reagents are abbreviated as follows: DMF: N,N-dimethylformamide PDA: p-phenylenediamine ODA: 4,4'-diaminodiphenyl ether m-TB: 4,4'-diamino-2,2'-dimethylbiphenyl BAPP: 2,2-bis[4-(4-aminophenoxy)phenyl]propane PMDA: pyromellitic dianhydride BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride BTDA: 3,3',4,4'-benzophenonetetracarboxylic dianhydride AA: acetic anhydride IQ: isoquinoline
[0110] [Preparation of Solution P1] 328.91 g of DMF, 11.85 g of ODA, and 11.17 g of m-TB were placed in a 2 L glass flask, and then 19.07 g of BTDA was gradually added to the flask while stirring the contents of the flask. After visually confirming that the BTDA had dissolved, 9.04 g of PMDA was gradually added to the flask while stirring the contents of the flask. After visually confirming that the PMDA had dissolved, the contents of the flask were stirred for an additional 30 minutes. Next, while stirring the contents of the flask, 2.13 g of PDA was added to the flask, followed by 5.88 g of PMDA, and the contents of the flask were stirred for an additional 30 minutes. Next, while stirring the contents of the flask, a previously prepared PMDA solution (solvent: DMF, dissolved amount of PMDA: 0.86 g, PMDA concentration: 7.2 wt %) was added to the flask for a predetermined time at an addition rate that did not cause a sudden increase in the viscosity of the flask content. When the viscosity of the flask content at a temperature of 23° C. reached 2,000 poise, the addition of the PMDA solution and stirring of the flask content were stopped, thereby obtaining Solution P1, a non-thermoplastic polyamic acid solution.
[0111] [Preparation of Solution P2] 328.94 g of DMF, 9.19 g of ODA, and 13.92 g of m-TB were placed in a 2 L glass flask, and then 19.02 g of BTDA was gradually added to the flask while stirring the contents of the flask. After visually confirming that the BTDA had dissolved, 9.01 g of PMDA was gradually added to the flask while stirring the contents of the flask. After visually confirming that the PMDA had dissolved, the contents of the flask were further stirred for 30 minutes. Next, while stirring the contents of the flask, 2.13 g of PDA was added to the flask, followed by 5.87 g of PMDA, and the contents of the flask were further stirred for 30 minutes. Next, while stirring the contents of the flask, a previously prepared PMDA solution (solvent: DMF, dissolved amount of PMDA: 0.86 g, PMDA concentration: 7.2 wt %) was added to the flask for a predetermined time at an addition rate that did not cause a sudden increase in the viscosity of the flask content. When the viscosity of the flask content at a temperature of 23° C. reached 2,000 poise, the addition of the PMDA solution and stirring of the flask content were stopped, thereby obtaining Solution P2, a non-thermoplastic polyamic acid solution.
[0112] [Preparation of Solution P3] 328.81 g of DMF, 9.30 g of ODA, and 12.68 g of m-TB were placed in a 2 L glass flask, and then 19.24 g of BTDA was gradually added to the flask while stirring the contents of the flask. After visually confirming that the BTDA had dissolved, 9.26 g of PMDA was gradually added to the flask while stirring the contents of the flask. After visually confirming that the PMDA had dissolved, the contents of the flask were further stirred for 30 minutes. Next, while stirring the contents of the flask, 2.87 g of PDA was added to the flask, followed by 5.79 g of PMDA, and the contents of the flask were further stirred for 30 minutes. Next, while stirring the contents of the flask, a previously prepared PMDA solution (solvent: DMF, dissolved amount of PMDA: 0.87 g, PMDA concentration: 7.2 wt %) was added to the flask for a predetermined time at an addition rate that did not cause a sudden increase in the viscosity of the flask content. When the viscosity of the flask content at a temperature of 23° C. reached 2,000 poise, the addition of the PMDA solution and stirring of the flask content were stopped, thereby obtaining Solution P3, a non-thermoplastic polyamic acid solution.
[0113] [Preparation of Solution P4] 328.55 g of DMF, 9.52 g of ODA, and 11.53 g of m-TB were placed in a 2 L glass flask, and then 17.50 g of BTDA was gradually added to the flask while stirring the contents of the flask. After visually confirming that the BTDA had dissolved, 9.48 g of PMDA was gradually added to the flask while stirring the contents of the flask. After visually confirming that the PMDA had dissolved, the contents of the flask were stirred for an additional 30 minutes. Next, while stirring the contents of the flask, 3.67 g of PDA was added to the flask, followed by 7.41 g of PMDA, and the contents of the flask were stirred for an additional 30 minutes. Next, while stirring the contents of the flask, a previously prepared PMDA solution (solvent: DMF, dissolved amount of PMDA: 0.89 g, PMDA concentration: 7.2 wt %) was added to the flask for a predetermined time at an addition rate that did not cause a sudden increase in the viscosity of the flask content. When the viscosity of the flask content at a temperature of 23° C. reached 2,000 poise, the addition of the PMDA solution and stirring of the flask content were stopped, thereby obtaining Solution P4, a non-thermoplastic polyamic acid solution.
[0114] [Preparation of Solution P5] 326.01 g of DMF and 23.83 g of m-TB were placed in a 2 L glass flask, and 35.09 g of BTDA was gradually added to the flask while stirring the contents. After visually confirming that the BTDA had dissolved, the contents were stirred for an additional 30 minutes. Next, while stirring the contents of the flask, a previously prepared BTDA solution (solvent: DMF, dissolved amount of BTDA: 1.09 g, BTDA concentration: 7.2 wt %) was added to the flask for a predetermined period of time at a rate that did not cause a sudden increase in the viscosity of the flask contents. When the viscosity of the flask contents at 23°C reached 2,000 poise, the addition of the BTDA solution and stirring of the flask contents were stopped, yielding Solution P5, a non-thermoplastic polyamic acid solution.
[0115] [Preparation of Solution P6] 327.98 g of DMF, 9.99 g of ODA, and 9.08 g of m-TB were placed in a 2 L glass flask, and then 13.78 g of BTDA was gradually added to the flask while stirring the contents of the flask. After visually confirming that the BTDA had dissolved, 8.86 g of PMDA was gradually added to the flask while stirring the contents of the flask. After visually confirming that the PMDA had dissolved, the contents of the flask were stirred for an additional 30 minutes. Next, while stirring the contents of the flask, 5.39 g of PDA was added to the flask, followed by 11.97 g of PMDA, and the contents of the flask were stirred for an additional 30 minutes. Next, while stirring the contents of the flask, a previously prepared PMDA solution (solvent: DMF, dissolved amount of PMDA: 0.93 g, PMDA concentration: 7.2 wt %) was added to the flask for a predetermined time at an addition rate that did not cause a sudden increase in the viscosity of the flask content. When the viscosity of the flask content at a temperature of 23° C. reached 2,000 poise, the addition of the PMDA solution and stirring of the flask content were stopped, thereby obtaining Solution P6, a non-thermoplastic polyamic acid solution.
[0116] [Preparation of Solution P7] 328.14 g of DMF, 8.45 g of ODA, and 7.46 g of m-TB were placed in a 2 L glass flask, and then 20.39 g of BTDA was gradually added to the flask while stirring the contents of the flask. After visually confirming that the BTDA had dissolved, 1.38 g of PMDA was gradually added to the flask while stirring the contents of the flask. After visually confirming that the PMDA had dissolved, the contents of the flask were stirred for an additional 30 minutes. Next, while stirring the contents of the flask, 6.84 g of PDA was added to the flask, followed by 14.57 g of PMDA, and the contents of the flask were stirred for an additional 30 minutes. Next, while stirring the contents of the flask, a previously prepared PMDA solution (solvent: DMF, dissolved amount of PMDA: 0.92 g, PMDA concentration: 7.2 wt %) was added to the flask for a predetermined time at an addition rate that did not cause a sudden increase in the viscosity of the flask content. When the viscosity of the flask content at a temperature of 23° C. reached 2,000 poise, the addition of the PMDA solution and stirring of the flask content were stopped, thereby obtaining Solution P7, a non-thermoplastic polyamic acid solution.
[0117] [Preparation of Solution P8] 328.91 g of DMF, 5.27 g of ODA, and 16.20 g of BAPP were placed in a 2 L glass flask, and 8.48 g of BTDA was gradually added to the flask while stirring the contents of the flask. After visually confirming that the BTDA had dissolved, 7.17 g of PMDA was gradually added to the flask while stirring the contents of the flask. After visually confirming that the PMDA had dissolved, the contents of the flask were stirred for an additional 30 minutes. Next, while stirring the contents of the flask, 7.11 g of PDA was added to the flask, followed by 14.92 g of PMDA, and the contents of the flask were stirred for an additional 30 minutes. Next, while stirring the contents of the flask, a previously prepared PMDA solution (solvent: DMF, dissolved amount of PMDA: 0.86 g, PMDA concentration: 7.2 wt %) was added to the flask for a predetermined time at an addition rate that did not cause a sudden increase in the viscosity of the flask content. When the viscosity of the flask content at a temperature of 23° C. reached 2,000 poise, the addition of the PMDA solution and stirring of the flask content were stopped, thereby obtaining Solution P8, a non-thermoplastic polyamic acid solution.
[0118] [Preparation of Solution P9] 328.53 g of DMF and 17.70 g of ODA were placed in a 2 L glass flask, and then 18.01 g of BPDA was gradually added to the flask while stirring the contents of the flask. After visually confirming that the BPDA had dissolved, 4.00 g of PMDA was gradually added to the flask while stirring the contents of the flask. After visually confirming that the PMDA had dissolved, the contents of the flask were further stirred for 30 minutes. Next, while stirring the contents of the flask, 5.77 g of m-TB was added to the flask, followed by 2.21 g of PDA, followed by 11.42 g of PMDA, and the contents of the flask were further stirred for 30 minutes. Next, while stirring the contents of the flask, a previously prepared PMDA solution (solvent: DMF, dissolved amount of PMDA: 0.89 g, PMDA concentration: 7.2 wt %) was added to the flask for a predetermined time at an addition rate that did not cause a sudden increase in the viscosity of the flask content. When the viscosity of the flask content at a temperature of 23° C. reached 2,000 poise, the addition of the PMDA solution and stirring of the flask content were stopped, thereby obtaining Solution P9, a non-thermoplastic polyamic acid solution.
[0119] [Preparation of Solution P10] 328.64 g of DMF and 17.53 g of ODA were placed in a 2 L glass flask, and then 11.89 g of BPDA was gradually added to the flask while stirring the contents of the flask. After visually confirming that the BPDA had dissolved, 6.51 g of BTDA was gradually added to the flask while stirring the contents of the flask. After visually confirming that the BTDA had dissolved, 11.31 g of PMDA was gradually added to the flask while stirring the contents of the flask. After visually confirming that the PMDA had dissolved, the contents of the flask were stirred for an additional 30 minutes. Next, while stirring the contents of the flask, 5.72 g of m-TB was added to the flask, followed by 2.19 g of PDA, followed by 11.31 g of PMDA, and the contents of the flask were stirred for an additional 30 minutes. Next, while stirring the contents of the flask, a previously prepared PMDA solution (solvent: DMF, dissolved amount of PMDA: 0.88 g, PMDA concentration: 7.2 wt %) was added to the flask for a predetermined time at an addition rate that did not cause a sudden increase in the viscosity of the flask content. When the viscosity of the flask content at a temperature of 23° C. reached 2,000 poise, the addition of the PMDA solution and stirring of the flask content were stopped, thereby obtaining Solution P10, a non-thermoplastic polyamic acid solution.
[0120] [Preparation of Solution P11] 328.85 g of DMF and 17.21 g of ODA were placed in a 2 L glass flask, and then 19.17 g of BTDA was gradually added to the flask while stirring the contents of the flask. After visually confirming that the BTDA had dissolved, 3.89 g of PMDA was gradually added to the flask while stirring the contents of the flask. After visually confirming that the PMDA had dissolved, the contents of the flask were further stirred for 30 minutes. Next, while stirring the contents of the flask, 5.61 g of m-TB was added to the flask, followed by 2.14 g of PDA, followed by 11.10 g of PMDA, and the contents of the flask were further stirred for 30 minutes. Next, while stirring the contents of the flask, a previously prepared PMDA solution (solvent: DMF, dissolved amount of PMDA: 0.87 g, PMDA concentration: 7.2 wt %) was added to the flask for a predetermined time at an addition rate that did not cause a sudden increase in the viscosity of the flask content. When the viscosity of the flask content at a temperature of 23° C. reached 2,000 poise, the addition of the PMDA solution and stirring of the flask content were stopped, thereby obtaining a non-thermoplastic polyamic acid solution, Solution P11.
[0121] [Preparation of Solution P12] 673.24 g of DMF and 71.83 g of BAPP were placed in a 2 L glass flask, and 7.72 g of BPDA was gradually added to the flask while stirring the contents. After visually confirming that the BPDA had dissolved, 31.30 g of PMDA was gradually added to the flask while stirring the contents. After visually confirming that the PMDA had dissolved, the contents of the flask were further stirred for 30 minutes. Next, while stirring the contents of the flask, a previously prepared PMDA solution (solvent: DMF, dissolved amount of PMDA: 1.15 g, PMDA concentration: 7.2 wt%) was continuously added to the flask for a predetermined period of time at an addition rate that did not cause a sudden increase in the viscosity of the flask contents. When the viscosity of the flask contents at 23°C reached 300 poise, the addition of the PMDA solution and stirring of the flask contents were stopped, yielding Solution P12, a thermoplastic polyamic acid solution.
[0122] Table 2 shows the diamines and their charge ratios used, as well as the acid dianhydrides and their charge ratios used for solutions P1 to P12. In Table 2, a "-" indicates that the corresponding component was not used. In Table 2, the values in the "Diamine" column represent the content (unit: mol%) of each diamine relative to the total amount of diamines used (100 mol%). In Table 2, the values in the "Acid Dianhydride" column represent the content (unit: mol%) of each acid dianhydride relative to the total amount of acid dianhydrides used (100 mol%). For each of solutions P1 to P12, the molar fraction of each polyamic acid residue in the prepared polyamic acid solution matched the molar fraction of each monomer (diamine and tetracarboxylic dianhydride) used in the synthesis of the polyamic acid.
[0123]
[0124] <Preparation of Polyimide Film> Hereinafter, the methods for preparing the polyimide films (specifically, the non-thermoplastic polyimide films and multilayer polyimide films) of Examples 1 to 6 and Comparative Examples 1 to 5 will be described.
[0125] Example 1 (Preparation of Non-Thermoplastic Polyimide Film) 24.0 g of an imidization accelerator consisting of AA / IQ / DMF (weight ratio: AA / IQ / DMF = 8.06 / 3.77 / 12.17) was added to 60.0 g of Solution P1 to prepare a dope solution. The dope solution was then degassed while stirring in an atmosphere at a temperature of 0°C or below, and then coated onto aluminum foil using a comma coater to form a coating film. The coating film was then heated at 110°C for 150 seconds to obtain a self-supporting gel film. The resulting gel film was peeled from the aluminum foil, fixed to a metal frame, and heated at 250°C for 17 seconds, followed by heating at 350°C for 70 seconds to dry and imidize, yielding a 17.0 μm-thick non-thermoplastic polyimide film (the non-thermoplastic polyimide film of Example 1).
[0126] (Preparation of multilayer polyimide film) 24.0 g of an imidization accelerator consisting of AA / IQ / DMF (weight ratio: AA / IQ / DMF = 8.06 / 3.77 / 12.17) was added to 60.0 g of solution P1 to prepare a dope solution (hereinafter referred to as "dope solution D1"). Next, dope solution D1 was degassed while stirring in an atmosphere at a temperature of 0 ° C or less. Next, using a comma coater, each solution was applied to aluminum foil in the order of solution P12 / dope solution D1 / solution P12 to form a three-layer coating film. Next, the coating film was heated at a heating temperature of 120 ° C for 200 seconds to obtain a self-supporting gel film. The obtained gel film was peeled off from the aluminum foil, fixed to a metal frame, and heated at 250°C for 17 seconds, and then at 350°C for 70 seconds to dry and imidize it, thereby obtaining a multilayer polyimide film (the multilayer polyimide film of Example 1) having a three-layer structure of a thermoplastic polyimide layer (thickness 4.0 μm) / a non-thermoplastic polyimide layer (thickness 17.0 μm) / a thermoplastic polyimide layer (thickness 4.0 μm).
[0127] [Examples 2 to 6 and Comparative Examples 1 to 5] Polyimide films (specifically, non-thermoplastic polyimide films and multilayer polyimide films) of Examples 2 to 6 and Comparative Examples 1 to 5 were obtained in the same manner as in Example 1, except that the type of solution (non-thermoplastic polyamic acid solution) was as shown in Table 3. In each of Examples 2 to 6 and Comparative Examples 1 to 5, the amount of non-thermoplastic polyamic acid solution used when producing the non-thermoplastic polyimide film and multilayer polyimide film was 60.0 g.
[0128] <Results> For Examples 1 to 6 and Comparative Examples 1 to 5, the types of solutions (non-thermoplastic polyamic acid solutions) used, the physical properties of the non-thermoplastic polyimide films, and the evaluation results of the desmear solution resistance of the multilayer polyimide films are shown in Table 3.
[0129]
[0130] In the multilayer polyimide films of Examples 1 to 6, the non-thermoplastic polyimide contained in the non-thermoplastic polyimide layer had a BTDA residue, which is a type of BENDA residue, and an m-TB residue, which is a type of BPDI residue. In the non-thermoplastic polyimide layer of Examples 1 to 6, the content of BPDI residue was 30 mol % or more and 100 mol % or less based on all diamine residues constituting the non-thermoplastic polyimide layer. Note that the non-thermoplastic polyimide contained in the non-thermoplastic polyimide layer of Examples 1 to 6 was a block copolymer having a specific segment.
[0131] As shown in Table 3, the evaluation results of the desmear solution resistance of the multilayer polyimide films of Examples 1 to 6 were A. Therefore, the multilayer polyimide films of Examples 1 to 6 were able to suppress a decrease in film strength due to the desmear treatment.
[0132] In the multilayer polyimide film of Comparative Example 1, the non-thermoplastic polyimide contained in the non-thermoplastic polyimide layer did not have a BPDI residue. In the multilayer polyimide film of Comparative Example 2, the non-thermoplastic polyimide contained in the non-thermoplastic polyimide layer did not have a BENDA residue. In the non-thermoplastic polyimide layers of Comparative Examples 2 to 5, the content of BPDI residues was less than 30 mol % relative to all diamine residues constituting the non-thermoplastic polyimide layers.
[0133] As shown in Table 3, the evaluation results of the desmear solution resistance of the multilayer polyimide films in Comparative Examples 1 to 5 were B or C. Therefore, the multilayer polyimide films in Comparative Examples 1 to 5 were unable to suppress the decrease in film strength due to the desmear treatment.
[0134] The above results demonstrate that the multilayer polyimide film according to the present invention can suppress a decrease in film strength due to desmear treatment.
[0135] 10: Multilayer polyimide film 11: Non-thermoplastic polyimide layer 12: Thermoplastic polyimide layer 13: Metal layer 20: Metal-clad laminate
Claims
1. A multilayer polyimide film having a non-thermoplastic polyimide layer and a thermoplastic polyimide layer disposed on at least one side of the non-thermoplastic polyimide layer, wherein the non-thermoplastic polyimide contained in the non-thermoplastic polyimide layer has tetracarboxylic dianhydride residues containing a benzophenone skeleton as the tetracarboxylic dianhydride residue and has diamine residues containing a biphenyl skeleton as the diamine residue, and the content of the diamine residues containing a biphenyl skeleton is 30 mol % or more and 100 mol % or less with respect to all diamine residues constituting the non-thermoplastic polyimide.
2. The multilayer polyimide film according to claim 1, wherein the content of the tetracarboxylic dianhydride residues containing the benzophenone skeleton is 30 mol % or more and 100 mol % or less of all tetracarboxylic dianhydride residues constituting the non-thermoplastic polyimide.
3. The multilayer polyimide film according to claim 1, wherein the non-thermoplastic polyimide layer has a strain retention rate of 80% or more after a desmear treatment is performed under conditions of a treatment temperature of 70° C. and a treatment time of 5 minutes.
4. The multilayer polyimide film according to claim 1, wherein the non-thermoplastic polyimide layer has a tensile stress at 10% strain of 220 MPa or more.
5. The multilayer polyimide film according to claim 1, wherein the linear expansion coefficient of the non-thermoplastic polyimide layer is 5.0 ppm / K or more and 19.0 ppm / K or less.
6. A metal-clad laminate comprising the multi-layer polyimide film according to claim 1 and a metal layer disposed on the main surface of at least one of the thermoplastic polyimide layers of the multi-layer polyimide film.
Citation Information
Patent Citations
Multilayer polyimide film and method for manufacturing multilayer polyimide film
JP2017177601A
Rigid flexible substrate
JP2019204977A
Polyamide acid, polyimide, polyimide film, metal-clad laminate and circuit board
JP2023006387A
Metal-clad laminate, circuit board, electronic device and electronic apparatus
JP2023051810A
Polyimide laminate
JP2024066870A
Cited By
Polyimide laminate
JP2024066870A
Polyimide film and laminate comprising same
JP2026087661A
Polyimide film and laminate containing the same
JP7897914B2