R-t-b sintered magnet

By controlling the two-grain boundary thickness distribution and optimizing the composition of RTB-based sintered magnets, the challenges of maintaining high coercive force and reducing heavy rare earth element usage are addressed, resulting in improved magnetic properties and reduced reliance on scarce materials.

WO2024203404A1PCT designated stage expired Publication Date: 2024-10-03PROTERIAL LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010079
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-14
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

RTB-based sintered magnets face challenges in maintaining high coercive force (HcJ) while minimizing the use of heavy rare earth elements like Dy, which are scarce and volatile in supply, and in achieving uniform grain boundary thickness for improved magnetic properties.

Method used

The development of an RTB-based sintered magnet with a controlled two-grain boundary thickness distribution, achieved by optimizing the composition and processing conditions, including the use of elements like Al, Ga, and Cu, and reducing the heavy rare earth element content, to enhance coercive force and magnetic flux density.

Benefits of technology

This approach results in an RTB-based sintered magnet with improved coercive force and magnetic flux density, while reducing the reliance on scarce heavy rare earth elements and achieving a uniform grain boundary thickness for enhanced magnetic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010079_03102024_PF_FP_ABST
    Figure JP2024010079_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This R-T-B sintered magnet has a main phase that comprises multiple R2T14B compound particles, and a grain boundary phase that is located between multiple R2T14B compound particles and that includes a two-particle grain boundary and grain boundary triple junctions. In a frequency histogram of grain boundary width measured from N reference points included in the two-particle grain boundary in a cross section which includes the orientation direction of the R-T-B sintered magnet in the plane thereof, when class intervals are determined so that the sixth lowest class represents the mode, the total frequency of three classes, i.e., the first, second, and third lowest classes, is not more than 12% of the whole.
Need to check novelty before this filing date? Find Prior Art

Description

RTB system sintered magnet

[0001] The present application relates to an RTB based sintered magnet.

[0002] R-T-B based sintered magnets (R is at least one of the rare earth elements, T is Fe or Fe and Co, and B is boron) are known as the most high performance permanent magnets, and are used in a variety of motors, including those for electric vehicles (EV, HV, PHV, etc.), industrial equipment, and home appliances. R-T-B based sintered magnets are mainly composed of R 2 T 14 It is composed of a main phase made of a B compound and a grain boundary phase (hereinafter sometimes simply referred to as "grain boundary") located at the grain boundary portion of this main phase. 2 T 14 The B compound is a ferromagnetic phase with high magnetization.

[0003] RTB based sintered magnets have a coercive force H cJ (Hereinafter, simply referred to as "coercive force" or "H cJ Therefore, the R-T-B based sintered magnets used in electric vehicle motors in particular require high H cJ It is required to have the following.

[0004] In RTB based sintered magnets, R 2 T 14 When a part of the light rare earth elements (mainly Nd and / or Pr) contained in R in the B compound is replaced with a heavy rare earth element (mainly Dy and / or Tb), H cJ It is known that the H cJ will improve.

[0005] However, R 2 T 14 When the light rare earth elements in the B compound are replaced with heavy rare earth elements, the H of the R-T-B sintered magnet cJ While the residual magnetic flux density B r (Hereafter, simply "B rFurthermore, heavy rare earth elements, especially Dy, are scarce in terms of resources and are produced in limited areas, resulting in unstable supplies and large price fluctuations. For this reason, in recent years, users have been seeking to produce H alloys that use as few heavy rare earth elements as possible. cJ It is required to improve.

[0006] Patent Document 1 discloses an R-T-B rare earth sintered magnet with increased coercivity while reducing the Dy content. The composition of this sintered magnet is limited to a specific range in which the amount of B is relatively small compared to commonly used R-T-B alloys, and it also contains one or more metal elements M selected from Al, Ga, and Cu. As a result, R is present at the grain boundaries. 2 T 17 phase is generated, and this R 2 T 17 The transition metal-rich phase (R 6 T 13 By increasing the volume ratio of the M phase, cJ will improve.

[0007] High B while reducing the content of heavy rare earth elements r and high H cJ In order to realize an RTB based sintered magnet having this property, a technique for controlling the thickness of the two-particle grain boundary is being investigated.

[0008] Patent Document 2 describes an example of a method for measuring the thickness of a two-grain grain boundary.

[0009] International Publication No. 2013 / 008756 Japanese Patent Application Laid-Open No. 2019-015573

[0010] The thickness of the two-particle grain boundary in an R-T-B based sintered magnet is not uniform, but varies depending on the position. According to the inventors' investigations, the thickness distribution of such two-particle grain boundaries changes depending on the conditions of heat treatment and element diffusion in the process of manufacturing an R-T-B based sintered magnet, and it has been found that controlling the thickness distribution of the two-particle grain boundaries makes it possible to improve the quality of magnet products.

[0011] An embodiment of the present disclosure provides an RTB based sintered magnet having a two-grain boundary thickness distribution that can exhibit excellent magnetic properties.

[0012] The RTB based sintered magnet of the present disclosure provides the solutions described in the following items.

[0013] [Item 1] An R-T-B based sintered magnet (R is at least one rare earth element, and always contains at least one of Nd and Pr, T is Fe or Fe and Co, and B is boron), comprising a plurality of R 2 T 14 a main phase consisting of B compound particles; 2 T 14 and a grain boundary phase located between B compound particles and including a two-particle grain boundary and a grain boundary triple junction, wherein, in a frequency histogram of grain boundary widths measured from N reference points included in the two-particle grain boundary in a cross section that includes within its plane the orientation direction of the R-T-B based sintered magnet, when the class widths are determined so that the sixth class from the lowest class represents the most frequent value, the total frequency of the first, second, and third classes from the lowest class is 12% or less of the total.

[0014] [Item 2] The RTB based sintered magnet according to Item 1, wherein the cross section is at a position at a distance of 0.05 mm or more and 0.15 mm or less from the surface of the RTB based sintered magnet.

[0015] [Item 3] The R-T-B based sintered magnet according to Item 1 or 2, wherein the relationship [T] / 55.85>14×[B] / 10.8 holds, where [T] is the composition ratio of T expressed in mass % and [B] is the composition ratio of B expressed in mass %.

[0016] [Item 4] The R-T-B based sintered magnet according to any one of Items 1 to 3, wherein the total frequency of the first, second, and third lowest classes in the frequency histogram is 10% or less of the total.

[0017] [Item 5] The R-T-B based sintered magnet according to any one of Items 1 to 4, wherein the total frequency of the first, second, and third lowest classes in the frequency histogram is 3% or more of the total.

[0018] [Item 6] The RTB based sintered magnet according to any one of Items 1 to 5, wherein the composition ratio of R in the RTB based sintered magnet is 31 mass % or less.

[0019] [Item 7] The RTB based sintered magnet according to any one of Items 1 to 6, wherein the total composition ratio of Dy and Tb in the RTB based sintered magnet is 0.5 mass % or less (including 0 mass %).

[0020] [Item 8] The RTB based sintered magnet according to any one of items 1 to 7, which includes a portion where the R concentration gradually decreases from the magnet surface toward the magnet interior.

[0021] [Item 9] The RTB based sintered magnet according to any one of Items 1 to 8, wherein the frequency of grain boundary widths of 0.03 μm or less in the frequency histogram is 12% or less overall.

[0022] [Item 10] An R-T-B based sintered magnet (R is at least one rare earth element, and always contains at least one of Nd and Pr, T is Fe or Fe and Co, and B is boron), comprising a plurality of R 2 T 14 a main phase consisting of B compound particles; 2 T 14 and a grain boundary phase located between B compound grains, the grain boundary phase including a two-particle grain boundary and a grain boundary triple junction, wherein in a frequency histogram of grain boundary widths measured from N reference points included in the two-particle grain boundary in a cross section that includes, in-plane, the orientation direction of the R-T-B based sintered magnet, the frequency of the grain boundary width being 0.03 μm or less is 12% or less overall.

[0023] [Item 11] The RTB based sintered magnet according to Item 10, wherein the cross section is at a position at a distance of 0.05 mm or more and 0.15 mm or less from the surface of the RTB based sintered magnet.

[0024] [Item 12] The R-T-B based sintered magnet according to Item 10 or 11, wherein the relationship [T] / 55.85>14×[B] / 10.8 holds, where [T] is the composition ratio of T expressed in mass % and [B] is the composition ratio of B expressed in mass %.

[0025] [Item 13] The RTB based sintered magnet according to any one of Items 10 to 12, wherein the frequency of the grain boundary width in the range of 0.02 μm or more and 0.03 μm or less in the frequency histogram is 5% or less overall.

[0026] [Item 14] The R-T-B based sintered magnet according to any one of Items 10 to 13, wherein the frequency of the grain boundary width in the range of 0.02 μm or more and 0.03 μm or less in the frequency histogram is 0.5% or more and 5% or less of the total.

[0027] [Item 15] The RTB based sintered magnet according to any one of Items 10 to 14, wherein the frequency histogram shows that the grain boundary width is 0.03 μm or less at a frequency of 3% to 12%.

[0028] [Item 16] An RTB based sintered magnet according to any one of Items 10 to 15, wherein the composition ratio of R in the RTB based sintered magnet is 31 mass % or less.

[0029] [Item 17] The R-T-B based sintered magnet according to any one of Items 10 to 16, wherein the total composition ratio of Dy and Tb in the R-T-M based sintered magnet is 0.5 mass % or less (including 0 mass %).

[0030] [Item 18] An RTB based sintered magnet according to any one of items 10 to 17, which includes a portion where the R concentration gradually decreases from the magnet surface toward the magnet interior.

[0031] [Item 19] The R-T-B based sintered magnet according to any one of Items 10 to 18, wherein, when the range of classes in the frequency histogram is determined so that the sixth to sixth classes represent the mode, the total frequency of the first, second, and third classes from the lowest class is 12% or less of the total.

[0032] According to the embodiments of the present disclosure, it is possible to provide an RTB based sintered magnet having a two-particle grain boundary thickness distribution that can exhibit excellent magnetic properties.

[0033] 1B is a schematic diagram showing the main phase and grain boundary phase of an R-T-B based sintered magnet. 1C is a schematic diagram further enlarged from the dashed rectangular region in FIG. 1A. 1D is a flowchart showing an example of a method for measuring the distribution of the thickness (grain boundary width) of two-grain grain boundaries in the cross section of an R-T-B based sintered magnet in an embodiment of the present disclosure. 1E is a diagram showing an example of a digital image of a backscattered electron image acquired from the cross section of an R-T-B based sintered magnet. 1F is a diagram showing a binarized image of the digital image of FIG. 3A. 1F is an enlarged view of a portion of the digital image of FIG. 3A. 1F is a diagram showing an image obtained by binarizing the digital image of FIG. 4A. 1F is a diagram showing a thinned image of the grain boundary phase generated from the binarized image of the grain boundary phase. 1F is a diagram showing an example of a thinned image of a two-grain grain boundary. 1F is a diagram showing an example of a reference point superimposed on a digital image before binarization. 1F is an enlarged view of a portion of FIG. 4E. 1F is a diagram showing an example of the direction (arrow) in which the grain boundary width is measured from a reference point (reference pixel) of interest. 1F is a diagram showing a measurement method extending from each of a plurality of reference pixels. 1 is a semi-logarithmic graph showing the relationship between the brightness value of each pixel expressed as a numerical value from 0 to 255 and the number of pixels showing each brightness value. It is a diagram showing an arbitrary position Q on a digital image and the brightness values ​​of four pixels surrounding position Q. It shows a frequency histogram showing the relationship between the measured value of grain boundary width and the measurement frequency (frequency or frequency of measurement) obtained by measuring the grain boundary width at multiple positions in the two-particle grain boundary in backscattered electron images obtained from the cross sections of each of the examples and comparative examples of the R-T-B based sintered magnet. C in the frequency histograms obtained from the examples and comparative examples of the present disclosure 1-3 Total frequency and H cJ 1 is a graph showing the relationship between the frequency (C3 frequency) of class C3 (grain boundary width in the range of 0.02 μm or more and 0.03 μm or less) and H in the frequency histograms obtained from the examples and comparative examples of the present disclosure. cJ 10 is a graph showing the relationship between

[0034] Conventionally, in an R-T-B based sintered magnet, for example, when (1) the content of R (at least one of rare earth elements, which necessarily includes at least one of Nd and Pr) is 27% by mass or more and 34% by mass or less of the entire R-T-B based sintered body, (2) T is Fe or Fe and Co, T always contains Fe, and the content of Fe relative to the entire T is 80% by mass or more, and (3) the molar ratio of T to B ([T] / [B]) is more than 14.0 and 15.0 or less, an element such as Ga is added to thicken the two-particle grain boundary and increase H. cJ It is known that this can improve

[0035] The molar ratio of T to B ([T] / [B]) is the ratio (a / b) of the number of moles (a) obtained by dividing the analytical value (mass %) of the concentration of each element (Fe and at least one of Co, Al, Mn, and Si) constituting T by the atomic weight of each element, to the number of moles (b) obtained by dividing the analytical value (mass %) of the concentration of B by the atomic weight of B.

[0036] The molar ratio of T to B ([T] / [B]) exceeding 14.0 means that the content ratio of B is R 2 T 14 In this case, in the R-T-B based sintered magnet, the main phase (R 2 T 14 The amount of B is relatively small compared to the amount of T used to form the hydroxyl group (B compound).

[0037] Next, the basic structure of an RTB based sintered magnet will be described.

[0038] RTB based sintered magnets have a structure in which powder particles of raw material alloys are bonded by sintering, and are mainly composed of R 2 T 14 It is composed of a main phase made of a B compound and a grain boundary phase located at the grain boundary of this main phase.

[0039] FIG. 1A is a schematic diagram showing the main phase and grain boundary phase of an R-T-B based sintered magnet, and FIG. 1B is a further enlarged schematic diagram of the dashed rectangular area in FIG. 1A. In FIG. 1A, an arrow of 5 μm in length is shown as an example for reference, showing the reference length of the size. As shown in FIGS. 1A and 1B, an R-T-B based sintered magnet is mainly composed of R 2 T 14 The grain boundary phase 14 is composed of a main phase 12 made of a B compound and a grain boundary phase 14 located at the grain boundary of the main phase 12. As shown in FIG. 1B, the grain boundary phase 14 is composed of two R 2 T 14 Two-particle grain boundary phase 14a in which B compound particles (grains) are adjacent, and three or more R 2 T 14 The B compound grains include adjacent grain boundary triple junctions 14b present around them.

[0040] R which is the main phase 12 2 T 14 The B compound is a ferromagnetic phase with high saturation magnetization and anisotropic magnetic field. 2 T 14 By increasing the proportion of B compounds, r It is possible to improve R 2 T 14 In order to increase the abundance ratio of B compounds, the amounts of R, T, and B in the raw alloy are adjusted to R 2 T 14 It is sufficient to approach the stoichiometric ratio of the B compound (R amount:T amount:B amount=2:14:1). 2 T 14 When the amount of B or R for forming the B compound is less than the stoichiometric ratio, the grain boundary phase 14 generally contains an Fe phase or an R phase. 2 T 17 soft magnetic phases such as H cJ However, the amount of B decreases sharply. 2 T 14 When the amount of B compound is less than the stoichiometric ratio and one or more metal elements M selected from Al, Ga, and Cu are contained, R 2 T 17 Instead of the phase, a transition metal-rich phase (e.g., RT-Ga phase) is generated at the grain boundary, and the two-grain grain boundary thickens, resulting in a high HcJ can be obtained.

[0041] As mentioned above, in an R-T-B based sintered magnet, the thickness of the two-particle grain boundary is not uniform even within the same field of view obtained by, for example, scanning electron microscope (SEM) observation, but varies depending on the location. The thickness of the two-particle grain boundary can have different values ​​depending on the measurement position. Measurement values ​​obtained by measuring the thickness of the two-particle grain boundary at multiple positions show a spread around the average value. According to the inventors' investigations, even in R-T-B based sintered magnets with the same average thickness of the two-particle grain boundary, the coercive force H cJ was found to be different.

[0042] First, we will explain an example of a method for determining the thickness distribution of two-grain grain boundaries in an R-T-B based sintered magnet. In this disclosure, the "thickness of two-grain grain boundaries" is a value measured in a cross section that includes the orientation direction of the R-T-B based sintered magnet within its plane (i.e., the cross section measured is not a cross section perpendicular to the orientation direction). Therefore, the "thickness" of a two-grain grain boundary that spreads three-dimensionally is equivalent to the "width" of the two-grain grain boundary that appears in such a cross section. Therefore, for simplicity, hereinafter, the "thickness of two-grain grain boundaries" may be referred to as the "grain boundary width." Note that the "orientation direction" of an R-T-B based sintered magnet is approximately parallel to the easy axis of magnetization (direction of easy magnetization) of the main phase crystals oriented in a magnetic field. R 2 T 14 The easy axis of magnetization of the B compound roughly coincides with the "c-axis" of this crystal. Therefore, the "orientation direction" of an RTB based sintered magnet is determined as the single direction in which the c-axes of the main phase crystal grains are most aligned.

[0043] An example of a method for measuring the distribution of grain boundary widths will be described in detail with reference to the flowchart of FIG.

[0044] First, an R-T-B based sintered magnet is prepared. Here, R is at least one rare earth element and always contains at least one of Nd and Pr, T is Fe or Fe and Co, and B is boron. As described above, an R-T-B based sintered magnet is made of a plurality of R 2 T 14 A main phase consisting of B compound particles and a plurality of R 2 T 14The grain boundary phase is located between the B compound grains and includes two grain boundaries and grain boundary triple junctions.

[0045] Next, in step S10 of FIG. 2 , a backscattered electron (BSE) image is obtained from the cross section of the R-T-B based sintered magnet using a scanning electron microscope (SEM). SEM imaging conditions include, for example, setting the magnification so that the pixel size is approximately 0.005 to 0.02 μm. Typically, the observation magnification is 3000 to 10000 times, the electron beam acceleration voltage is 1 to 5 kV, and the current value is 15 to 20 μA. To obtain more accurate data, it is desirable to use a field emission scanning electron microscope (FE-SEM). The composition range and manufacturing method of the R-T-B based sintered magnet in this embodiment will be described later. The cross section of the R-T-B based sintered magnet is a cross section that includes the orientation direction of the R-T-B based sintered magnet within the plane.

[0046] In step S11, digital data (grayscale) of the backscattered electron image is generated. FIG. 3A shows an image of the digital data. In the digital image of FIG. 3A, the main phase is represented by pixels with relatively low brightness values ​​and is observed as a black area. In contrast, the grain boundary phase is represented by pixels with relatively high brightness values ​​and is observed as gray or white. The brightness value increases as the signal intensity of the backscattered electrons increases, and the signal intensity of the backscattered electrons increases as the concentration of elements with a larger atomic number Z increases. In an 8-bit grayscale image, the brightness value of each pixel is expressed in 256 levels, from 0 to 255.

[0047] In an embodiment of the present disclosure, the surface on which a digital backscattered electron image is captured is at a depth of 0.05 mm to 0.15 mm from the magnet surface. The surface to be captured may be prepared using a known processing device and processing method. For example, the sample may be cut with a peripheral blade cutter to obtain a cross section that includes the orientation direction within the surface, the cross section may be appropriately smoothed with sandpaper, and finally a cross-section polisher may be used to prepare a smooth, clean sample cross section that is free of processing distortion or sagging. The area of ​​the digital image (capture area) is 100 μm when acquiring one digital image. 2 It is preferable that the thickness is 400 μm or more. 2 For example, an area having a size of 20 μm or more in the horizontal direction and 20 μm or more in the vertical direction can be imaged. In addition, multiple digital images can be taken from one R-T-B based sintered magnet, and a total of 3000 μm can be obtained. 2 The plurality of digital images are acquired by either capturing digital images at random or capturing a cross section in a manner that connects the plurality of digital images.

[0048] Next, in step S12 of FIG. 2 , binary images of the main phase and the grain boundary phase are extracted from the digital image. Specifically, the digital image of FIG. 3A is binarized to generate the binary image shown in FIG. 3B . In this example, among the numerous pixels constituting the digital image, the grain boundary phase is represented by black pixels, and the main phase is represented by relatively bright pixels (gray pixels in the figure, but typically "white" pixels). More specifically, when generating a binary digital image from a backscattered electron image, each pixel constituting the image before binarization is classified as either a "grain boundary phase" or a "main phase" based on its brightness value. Whether a pixel is classified as a "grain boundary phase" is determined by whether its brightness value is higher than a predetermined threshold. As will be described later, depending on the magnitude of this threshold, a pixel with an intermediate brightness value in the digital image before binarization may be classified as either a "grain boundary phase" or a "main phase" in the binarized image. This indicates that the shape and size of the grain boundary phase in the binarized image may change depending on the magnitude of the threshold. However, in the embodiment of the present disclosure, the binarized image is used to generate a thinned image of the two-particle grain boundary, and the grain boundary width is measured based on the grayscale image before binarization, which prevents the measured value of the grain boundary width from fluctuating greatly depending on the threshold value.

[0049] Fig. 4A is an enlarged view of a portion of the digital image (grayscale image) in Fig. 3A. The enlarged region will be described below, and the following processing is performed on five images having a size of, for example, about 10 μm × 10 μm selected from the digital image, which corresponds to a field of view of, for example, 28 μm × 21 μm in the imaged cross section.

[0050] In the digital image of Fig. 4A, the areas with relatively high brightness correspond to the grain boundary phase. Fig. 4B is a binarized image of the digital image of Fig. 4A. The binarized image of the grain boundary phase is indicated by black pixels.

[0051] In step S13 shown in FIG. 2, a thinned image of the grain boundary phase is generated from the binary image of the grain boundary phase. Thinning can be performed by any image processing technique. An example of the generated "thinned image of the grain boundary phase" is shown in FIG. 4C. The line width of the thinned image of the two-particle grain boundary corresponds to the width of one pixel. Each pixel constituting such a thinned image forms a "continuous thin line" by being adjacent to at least one of the eight pixels located around it.

[0052] In step S14, the grain boundary triple junction is removed from the grain boundary phase thinning image to generate a two-particle grain boundary thinning image. An example of a two-particle grain boundary thinning image is shown in FIG. 4D. The method for removing the grain boundary triple junction is not limited to a specific method, but the method described in Patent Document 2, for example, can be used. The entire contents of JP 2019-015573 A are incorporated herein by reference.

[0053] In step S15, positions on the digital image before binarization corresponding to each of N pixels (N is an integer equal to or greater than 10,000, for example) constituting the thinned image of the two-particle grain boundary are set as N reference points, and the grain boundary width is measured from each of the N reference points. FIG. 4E shows an example of reference points superimposed on the digital image before binarization. FIG. 4F is an enlarged view of a portion of FIG. 4E. In FIG. 4E, the region where pixels with relatively high brightness are concentrated indicates the grain boundary phase. A pixel with low brightness located near the center in the direction in which the "width" of the grain boundary phase expands (thickness direction of the grain boundary phase) corresponds to the reference point. Each reference point is a pixel constituting the thinned image of the two-particle grain boundary.

[0054] To measure the grain boundary width from each reference point, it is necessary to estimate the direction in which the grain boundary phase expands toward the main phase on both sides of the grain boundary phase (thickness direction of the grain boundary phase). Figure 4G shows an arrow indicating the direction in which the grain boundary width is measured from a reference point (reference pixel) of interest. The measurement direction (direction of the double-headed arrow) is determined, for example, so as to be perpendicular to the line segment connecting the centers of two pixels adjacent to the reference pixel of interest. In this case, each of the two pixels adjacent to the reference pixel of interest is one of the eight neighboring pixels of the reference pixel. Note that the measurement direction determined in this manner may vary slightly depending on the position of the reference pixel, so the average direction of multiple consecutive reference pixels (e.g., five or seven) may be selected as the measurement direction. Furthermore, the two tips of each double-headed arrow shown in Figures 4G and 4H are located at the boundary between the grain boundary phase and the main phase. In other words, the length of each double-headed arrow is the "grain boundary width" at the position of that double-headed arrow (the position of the corresponding reference point).

[0055] To accurately measure the grain boundary width along the measurement direction determined by the above method, it is necessary to determine the positions of the arrowheads extending from each reference point shown in Figure 4H with high positional resolution. In the digital image before binarization shown in Figure 4H, similar to the image of Figure 3A, the brightness value of each pixel has a value of, for example, 0 to 255. For example, as can be seen from the image of Figure 3A, the brightness value of the grain boundary phase is higher than that of the main phase. By selecting an appropriate brightness value intermediate between the brightness values ​​of the grain boundary phase and the main phase as the reference value for classification, pixels whose brightness values ​​are equal to or greater than the reference value can be classified as grain boundary phase.

[0056] 5 is a semi-logarithmic graph showing the relationship between the brightness value of each pixel expressed in gradations of 0 to 255 and the number of pixels showing each brightness value in the digital image (grayscale image) shown in FIG. 3A, for example. The horizontal axis of the graph is the brightness value, and the vertical axis is logarithmic. 10 5, local modes are observed around brightness values ​​of approximately 60, 110, 130, 170, and 180, and the pixels with a brightness value of approximately 60 are determined to be the main phase, the pixels with a brightness value of approximately 110 are determined to be the R-T-Ga phase, and the pixels with a brightness value of approximately 170 are determined to be the oxide phase.

[0057] When digital images (grayscale images) are generated from each of multiple backscattered electron images acquired from the cross section of an R-T-B based sintered magnet, the brightness values ​​in each digital image exhibit a distribution roughly shown in FIG. 5. However, the positions of local peaks in brightness values ​​may vary depending on the imaging conditions. For this reason, in the present disclosure, gamma correction is performed on the digital image before binarization, thereby calibrating the image so that the position of the local peak in brightness values ​​in the main phase (value on the horizontal axis) indicates a value of 60, and the position of the local peak in brightness values ​​in the oxide phase within the grain boundary phase (value on the horizontal axis) indicates a value of 170. FIG. 5 shows an example of the frequency (frequency) distribution of brightness values ​​in this gamma-corrected digital image (before binarization).

[0058] In the present disclosure, a brightness value of 85 is adopted for the grayscale image after the gamma correction as an appropriate reference value intermediate between the brightness value of the grain boundary phase and the brightness value of the main phase. That is, when the digital image (grayscale image) after the gamma correction is binarized, a brightness value of 85 is used as the reference value. Specifically, pixels with a brightness value of 85 or more are classified as the grain boundary phase, and pixels with a brightness value of less than 85 are classified as the main phase.

[0059] The brightness value is obtained pixel by pixel from a digital image (grayscale image). Therefore, if the size of one pixel is, for example, 0.01 μm (=10 nm), the measurable "grain boundary width resolution" is 0.01 μm. To measure the grain boundary width with high precision, it is preferable to reduce the size of one pixel (for example, to less than 0.01 μm). In order to increase the position resolution regardless of the size of one pixel, linear interpolation is performed in this disclosure. An example of linear interpolation will be described below with reference to FIG. 6.

[0060] 6 shows an arbitrary position Q on a digital image and four pixels whose centers surround position Q. Specifically, four pixels, 2 pixels horizontally and 2 pixels vertically, are shown, and a rectangle connecting the centers of the pixels surrounds position Q. Here, the positions of the four pixels (center positions of each pixel) are represented by (j, k), (j+1, k), (j, k+1), and (j+1, k+1), and the luminance values ​​at the center positions of each pixel are represented by R(j, k), R(j+1, k), R(j, k+1), and R(j+1, k+1). If the horizontal and vertical sizes of one pixel are Px and Py, respectively, the luminance value at position Q can be approximated by an interpolation technique such as bilinear interpolation based on R(j, k), R(j+1, k), R(j, k+1), R(j+1, k+1), and dx / Px and dy / Py that define the relative position of point Q among the four pixels. When the luminance value of each pixel is given in this way, the position where the luminance value is equal to 85, i.e., the position of the boundary between the grain boundary phase and the main phase, can be determined without being limited by the pixel size.

[0061] Once the position (boundary position) where the brightness value is equal to 85 is determined in this manner, the distance from each reference point to the boundary position along the measurement direction described above is calculated. Since each reference point is sandwiched between two boundaries, a single measurement value of the grain boundary width is obtained by adding the distances from the reference point to each boundary located on both sides of the reference point of interest. The reference points are preferably all of the pixels that make up the thinned image of the two-particle grain boundary of the grain boundary phase, but they may also be selected at predetermined intervals so as to skip some pixels, for example. The number N of reference points selected from one digital image is preferably 10,000 or more.

[0062] Referring again to Fig. 2, in step S16, a frequency histogram is created for the grain boundary widths measured based on the digital image (grayscale image), with the sixth to sixth classes representing the most frequent values. At this time, the class widths are set to be constant.

[0063] Fig. 7 shows frequency histograms illustrating the relationship between the grain boundary width measurements, obtained by measuring the grain boundary width at multiple positions within a two-particle grain boundary, and the measurement frequency (frequency or frequency of measurements) in backscattered electron images taken from the cross sections of each of the example and comparative examples of R-T-B based sintered magnets. In Fig. 7, classes are separated by multiple vertically extending dashed lines, and the lowest class C1 through the Xth class are marked with the symbol "CX." The width of a class is the distance between two adjacent dashed lines.

[0064] In this frequency histogram, the width of the classes on the grain boundary width axis is determined so that the lowest class C1 to the sixth class C6 show the most frequent value (mode) M. In FIG. 7, data for the Examples are shown by squares, and data for the Comparative Examples are shown by triangles. The distinguishing feature between the Examples and the Comparative Examples is that the total frequency of the three classes C1, C2, and C3, from the lowest class C1 to the first, second, and third classes, is 12% or less of the total. Hereinafter, the total of these three classes will be referred to as "C 1-3 According to the grain boundary width measurement method described above, the total class C 1-3 is defined by a grain boundary width of 0.03 μm or less (a range of more than 0 μm and less than 0.03 μm). Note that deviations in the measured values ​​of the grain boundary width may occur depending on how the grain boundary width is measured. However, even if such deviations occur, the influence of the deviations can be ignored if the class widths are determined so that the lowest class C1 to the sixth class C6 show the mode M.

[0065] As will be understood from the explanations of the Examples and Comparative Examples described later, the total frequency (C 1-3 In the R-T-B based sintered magnets (Examples) where the total frequency is 12% or less, H cJ C can achieve excellent values ​​of about 1400 kA / m or more, typically about 1500 kA / m or more. 1-3 The lower the ratio of the total frequency (especially the frequency of class C3) to the whole, the higher the H cJ This indicates that the thickness distribution of the two-grain grain boundary and H cJ The relationship between these two properties will be clarified, and guidelines for grain boundary modification will be provided.

[0066] Hereinafter, an example of an embodiment of a method for producing an R-T-B based sintered magnet in which the total frequency of the three classes C1, C2, and C3 is 12% or less of the total (the frequency of the grain boundary width being 0.03 μm is 12% or less of the total) will be described.

[0067] <RTB based sintered magnet> R is a rare earth element including Y and Sc, and must contain at least one element selected from the group consisting of Nd, Pr, and Ce. Preferably, a combination of rare earth elements represented by Nd-Pr, Nd-Dy, Nd-Tb, Nd-Dy-Tb, Nd-Pr-Dy, Nd-Pr-Tb, or Nd-Pr-Dy-Tb is used.

[0068] Among R, Dy and Tb are particularly cJ This is effective in improving the properties of the magnet. In addition to the above elements, other rare earth elements such as La and Ho may be contained, and misch metal or didymium may also be used. Furthermore, R does not need to be a highly pure element; it may contain impurities unavoidable during production as long as they are industrially available. The R content is, for example, 27% to 35% by mass. The R content of the R-T-B based sintered magnet is preferably 31% by mass or less (27% to 31% by mass, preferably 29% to 31% by mass). By controlling the R content of the R-T-B based sintered magnet to 31% by mass or less and the oxygen content to 400 ppm to 4000 ppm (preferably 400 ppm to 2500 ppm, more preferably 400 ppm to 2000 ppm), the generation of oxidized R is reduced. This allows for better magnetic properties to be obtained.

[0069] T contains iron (including cases where T consists essentially of iron (Fe)), and up to 50% by mass of iron may be substituted with cobalt (Co) (including cases where T consists essentially of iron and cobalt). Co is effective in improving temperature characteristics and corrosion resistance, and 10% by mass or less of Co may be contained. The content of T may account for the remainder of R and B, or R, B, and M, which will be described later.

[0070] The content of B may be a known content, and for example, a preferred range is 0.8 mass % to 1.2 mass %. If it is less than 0.8 mass %, high H cJIf it exceeds 1.2 mass%, B may not be obtained. r In addition, a part of B can be substituted with C (carbon).

[0071] In addition to the above elements, H cJ In order to improve the properties, an M element can be added. The M element is one or more elements selected from the group consisting of Al, Si, Ti, V, Cr, Mn, Ni, Cu, Zn, Ga, Zr, Nb, Mo, In, Sn, Hf, Ta, and W. The amount of the M element added is preferably 5.0 mass % or less. If it exceeds 5.0 mass %, B r In addition, unavoidable impurities can be tolerated.

[0072] The N (nitrogen) content in the R-T-B based sintered magnet is preferably 50 ppm or more and 600 ppm or less. By pulverizing the magnet so that the N (nitrogen) content is 50 ppm or more and 600 ppm or less, it is possible to improve pulverizability while suppressing the deterioration of magnetic properties due to nitriding. The nitrogen content is more preferably 50 ppm or more and 400 ppm or less, and most preferably 100 ppm or more and 300 ppm or less. This is because it is possible to further improve pulverizability while suppressing the deterioration of magnetic properties due to nitriding. Furthermore, the C (carbon) content in the R-T-B based sintered magnet is preferably 50 ppm or more and 1300 ppm or less.

[0073] An example of the composition of the R-T-B based sintered magnet in this embodiment is shown below: R: 28% by mass or more and 35% by mass or less, B: 0.8% by mass or more and 1.2% by mass or less, and T: 61.5% by mass or more, where the composition ratio of T expressed in mass% is [T] and the composition ratio of B expressed in mass% is [B], the following formula 1 is satisfied: [T] / 55.85>14×[B] / 10.8.

[0074] By satisfying the relational expression (1), the B content becomes smaller than that of a typical RTB based sintered magnet. 2 T 14 In addition to the B phase, there is a soft magnetic phase R that inhibits the improvement of coercivity. 2 T 17To prevent the formation of any phase, [T] / 55.85 (atomic weight of Fe) is less than 14×[B] / 10.8 (atomic weight of B).

[0075] <(1) Example of a Process for Preparing Coarsely Pulverized Powder of Alloy for R-T-B Based Sintered Magnet> In this embodiment, the process for preparing coarsely pulverized powder of alloy for R-T-B based sintered magnet can include a process for preparing an alloy for R-T-B based sintered magnet and a process for coarsely pulverizing this alloy by, for example, a hydrogen pulverization method.

[0076] The following is an example of a method for producing an alloy for an RTB based sintered magnet.

[0077] First, an alloy ingot can be obtained by ingot casting, in which a metal or alloy previously prepared to have the above-mentioned composition is melted and poured into a mold. Alternatively, the molten metal can be brought into contact with a single roll, twin rolls, rotating disk, or rotating cylindrical mold, etc., and quenched to produce alloy flakes by a quenching method, typically a strip casting method.

[0078] In embodiments of the present disclosure, materials produced by either the ingot method or the quenching method can be used, but production by a quenching method such as strip casting is preferred. The thickness of quenched alloys produced by the quenching method is typically in the range of 0.03 mm to 1 mm and is in the form of flakes. The molten alloy begins to solidify from the surface that contacts the chill roll (the roll contact surface), and crystals grow columnarly from the roll contact surface in the thickness direction. Compared to alloys (ingot alloys) produced by conventional ingot casting (mold casting), quenched alloys are cooled in a shorter time, resulting in a moderately refined structure and small crystal grain size. Because the R-rich phase spreads widely within the grain boundaries, the quenching method provides excellent dispersion of the R-rich phase. Therefore, they are prone to fracture at the grain boundaries when subjected to hydrogen pulverization. By subjecting the quenched alloy to hydrogen pulverization, the size (average particle size) of the hydrogen pulverized powder (coarsely pulverized powder) is reduced to, for example, 1.0 mm or less, preferably 10 μm to 500 μm, and the alloy is embrittled, making it easy to obtain a fine powder in the next step. The average particle size (d50) in this disclosure can be measured by an air-dispersion laser diffraction method (in accordance with JIS Z 8825: 2013 revised edition). That is, in this specification, the average particle size refers to the particle size (median diameter) at which the cumulative particle size distribution (volume basis) from the small particle size side is 50%.

[0079] <(2) Example of a Process for Obtaining Fine Powder> In the process for obtaining fine powder in this embodiment, for example, the coarsely pulverized powder is supplied to a jet mill device whose pulverization chamber is filled with an inert gas, and the coarsely pulverized powder is pulverized to obtain fine powder. In this process, for example, a fine powder (RTB-based alloy powder) having an average particle size of 2.0 μm or more and 8.0 μm or less can be obtained. The process for obtaining such fine powder can be carried out, for example, using a jet mill pulverization system.

[0080] The increase in oxygen content of the R-T-B based sintered magnet due to the processes after pulverization (mainly the process of producing a sintered body from the fine powder) is preferably 50 ppm to 300 ppm, more preferably 50 ppm to 200 ppm. To achieve this, as described below, it is preferable to perform wet pressing in a magnetic field or magnetic pressing in an inert gas atmosphere, and then sinter the resulting compact. The average particle size of the fine powder obtained in the process of obtaining the fine powder is preferably 2.0 μm to 5.0 μm, more preferably 2.5 μm to 4.0 μm. Reducing the average particle size makes it possible to improve magnetic properties. On the other hand, excessively reducing the average particle size leads to a decrease in productivity.

[0081] <(3) Example of a Process for Producing a Compact of Fine Powder> In the process for producing a compact, a magnetic field pressing is generally employed, in which the powder is inserted into a mold and pressed by applying a magnetic field from the outside. In the process for producing a compact, it is preferable to form the compact by pressing in an inert gas atmosphere or wet pressing from the viewpoint of suppressing oxidation when using magnetic field pressing. In particular, wet pressing coats the surfaces of the particles constituting the compact with a dispersant such as an oil, suppressing contact with oxygen or water vapor in the atmosphere. This makes it possible to prevent or suppress oxidation of the particles by the atmosphere before, during, or after the pressing process.

[0082] When wet pressing in a magnetic field is performed, a slurry is prepared by mixing fine powder with a dispersion medium, and the slurry is supplied to a cavity in a mold of a wet pressing device and pressed in a magnetic field to obtain a green body.

[0083] <(4) Example of Sintering Step> Next, the compact is sintered to obtain a sintered body. The sintering temperature is, for example, 900°C or higher and 1100°C or lower. The sintering step is not particularly limited and may be performed, for example, by a known method. The sintering step in this embodiment may be performed in a vacuum or in an inert gas such as helium or argon. After sintering, it is preferable to perform a further heat treatment. The heat treatment can improve the magnetic properties. Known conditions may be used for the heat treatment, such as the heat treatment temperature and heat treatment time.

[0084] The RTB based sintered magnet thus obtained is subjected to grinding and polishing steps, surface treatment steps, and magnetization steps as required, to complete the final RTB based sintered magnet.

[0085] The magnetic properties of the R-T-B based sintered magnet produced by the above process can be improved by diffusing various elements from the surface to the interior. In this case, the sintered body before diffusion can be called an "RTB based sintered magnet material."

[0086] The sintered R-T-B based magnet material may be produced from one type of raw material alloy (single raw material alloy), or may be produced by mixing two or more types of raw material alloys (blending method). Furthermore, the obtained sintered R-T-B based magnet material may be subjected to known mechanical processing such as cutting or milling, as necessary, and then subjected to the first and second heat treatments described below.

[0087] In this embodiment, a metal, alloy, compound, or the like containing at least one of Nd and Pr may be diffused from the surface toward the interior of the sintered R-T-B based magnet material obtained by the above method. As a result of such diffusion, the R-T-B based sintered magnet includes a portion where the Nd concentration and / or Pr concentration gradually decreases from the magnet surface toward the magnet interior. Similarly, a metal, alloy, compound, or the like containing at least one of Tb and Dy may be diffused from the magnet surface toward the magnet interior. As a result of such diffusion, the R-T-B based sintered magnet includes a portion where the Tb concentration and / or Dy concentration gradually decreases from the magnet surface toward the magnet interior.

[0088] Step of Preparing Diffusion Source First, the composition of the diffusion source in the step of preparing the diffusion source will be described.

[0089] The diffusion source may be composed of heavy rare earth elements such as Dy, Tb, Gd, and Ho, but preferably contains at least one of Nd and Pr as a rare earth element. It is preferable that 50 mass % or more of the rare earth elements is Pr. cJ According to the present disclosure, a sufficiently high HcJ Therefore, the content of the heavy rare earth element is preferably 10 mass % or less of the entire diffusion source, more preferably 5 mass % or less, and even more preferably none (substantially 0 mass %). Even when the diffusion source contains a heavy rare earth element, it is preferable that 50% or more of the rare earth element is Pr, and it is more preferable that the rare earth element excluding the heavy rare earth element is only Pr (including unavoidable impurities).

[0090] When at least one of Nd and Pr is necessarily contained as a rare earth element, the content thereof is preferably, for example, 35% by mass or more and less than 85% by mass of the entire diffusion source. If the content of the rare earth element is less than 35% by mass, there is a possibility that diffusion will not proceed sufficiently in the first heat treatment described below. On the other hand, if the content of the rare earth element is 85% by mass or more, the alloy powder becomes very active during the manufacturing process of the diffusion source. As a result, the alloy powder may be significantly oxidized or ignite.

[0091] In addition to the above elements, the diffusion source may contain Ga, Fe, Cu, Co, Al, Ag, Zn, Si, In, Sn, Zr, Nb, Ti, Ni, Hf, Ta, W, Ge, Mo, V, Y, La, Ce, Sm, Ca, Mg, Mn, Cr, H, F, P, S, Cl, O, N, C, etc.

[0092] The diffusion source can be prepared using a raw material alloy production method employed in common manufacturing methods typified by R-T-B based sintered magnets, such as die casting, strip casting, single-roll rapid cooling (melt spinning), or atomization. Alternatively, the diffusion source may be obtained by pulverizing the alloy obtained by the above method using a known pulverizing method such as a pin mill. Furthermore, to improve the pulverizability of the alloy obtained by the above method, the alloy may be subjected to a heat treatment at 700°C or less in a hydrogen atmosphere to incorporate hydrogen before pulverization.

[0093] A step of diffusing elements contained in the diffusion sources from the surface of the sintered R-T-B based magnet material into the interior. The elements contained in the diffusion sources are diffused from the surface of the sintered R-T-B based magnet material into the interior by heat treatment at a temperature of 700°C or higher and 1100°C or lower in a vacuum or inert gas atmosphere. In the present disclosure, this heat treatment is referred to as the first heat treatment. If the heat treatment temperature for diffusion is lower than 700°C, the diffusion will be insufficient, resulting in a high H cJ On the other hand, if the temperature exceeds 1100°C, abnormal grain growth of the main phase occurs, and H cJ The heat treatment temperature for diffusion is preferably 800°C or higher and 1000°C or lower. cJ This is because it is possible to obtain the above. The heat treatment time is set to an appropriate value depending on the composition and dimensions of the sintered body material and the diffusion source, the heat treatment temperature, etc., but is preferably 5 minutes to 30 hours, more preferably 10 minutes to 25 hours, and even more preferably 30 minutes to 20 hours. It is also preferable to prepare the diffusion source in an amount of 1 mass % to 30 mass % of the weight of the sintered body material. If the diffusion source is less than 1 mass % of the weight of the sintered body material, H cJ On the other hand, if it exceeds 30 mass %, B r may decrease.

[0094] The heat treatment for diffusion can be performed using a known heat treatment method. For example, the surface of the sintered R-T-B based magnet material can be covered with a powder layer of the diffusion source and then the first heat treatment can be performed. For example, the surface of the sintered R-T-B based magnet material can be coated with the diffusion source by sputtering, and then the first heat treatment can be performed. In this case, the diffusion source coated on the surface can have a multilayer structure composed of a layer of metal or alloy containing no rare earth and a layer of metal or alloy containing rare earth. For example, a slurry in which the diffusion source is dispersed in a dispersion medium can be applied to the surface of the sintered R-T-B based magnet material, and the dispersion medium can then be evaporated to bring the diffusion source and the sintered R-T-B based magnet material into contact. Examples of dispersion mediums include alcohol (e.g., ethanol), NMP (N-methylpyrrolidone), aldehydes, and ketones. Furthermore, the sintered R-T-B based magnet material that has undergone the first heat treatment can be subjected to known machining processes such as cutting or milling.

[0095] The R-T-B based sintered magnet material that has been subjected to the heat treatment for diffusion may be subjected to another heat treatment in a vacuum or inert gas atmosphere at a temperature of 450°C or higher and 600°C or lower. In the present disclosure, this heat treatment is referred to as the second heat treatment. By performing the second heat treatment, a high B r and high H cJ By setting the temperature of the second heat treatment to 450° C. or more and 600° C. or less, R 6 T 13 The formation of the Ga phase progresses (if the resulting sintered magnet contains Ga). The second heat treatment temperature is preferably 480°C or higher and 560°C or lower. cJ The heat treatment time can be set appropriately depending on the composition and dimensions of the sintered body material, the heat treatment temperature, etc. The heat treatment time is preferably 5 minutes to 20 hours, more preferably 10 minutes to 15 hours, and even more preferably 30 minutes to 10 hours.

[0096] The production of an R-T-B based sintered magnet in which the combined frequency of the first, second, and third lowest grades is 12% or less (the combined frequency of grain boundary widths of 0.03 μm or less is 12% or less) is determined by a balance between the magnet composition, sintering temperature, and heat treatment temperature. Furthermore, when diffusing at least one of Nd and Pr from the surface toward the interior of a sintered body material, the combined frequency is determined by a balance between the composition of the diffusion source, the amount of application, and the heat treatment temperature for diffusion. By examining these manufacturing conditions through experiments, etc., it is possible to produce an R-T-B based sintered magnet in which the combined frequency of the first, second, and third lowest grades is 12% or less (the combined frequency of grain boundary widths of 0.03 μm or less is 12% or less). The experimental examples described below show examples in which the post-sintering heat treatment temperature, the composition of the diffusion source, and the amount of application were adjusted.

[0097] Experimental Example: The raw materials for each element were weighed so that the R-T-B based sintered magnet material had the composition shown in Table 1, and alloys were produced by strip casting. Each of the resulting alloys was coarsely pulverized by hydrogen pulverization to obtain coarsely pulverized powder. Next, zinc stearate was added as a lubricant to the resulting coarsely pulverized powder in an amount of 0.04% by mass relative to 100% by mass of the coarsely pulverized powder, and the mixture was then dry-pulverized in a nitrogen stream using an airflow pulverizer (jet mill).

[0098] The finely pulverized powder was mixed with zinc stearate (0.05 mass % relative to 100 mass % of the finely pulverized powder) as a lubricant and compacted in a magnetic field to obtain a green body. The compacting device used was a so-called perpendicular magnetic field compacting device (horizontal magnetic field compacting device), in which the magnetic field application direction and the pressure direction are perpendicular to each other. The resulting green body was sintered in a vacuum at 1060°C to 1090°C (a temperature selected for each sample at which sufficient densification by sintering occurs) for 4 hours to obtain an R-T-B based sintered magnet. The density of the resulting R-T-B based sintered magnet material was 7.5 Mg / m 3 The results for the components of the obtained sintered RTB based magnet material are shown in Table 1. The components in Table 1 were measured using inductively coupled plasma optical emission spectroscopy (ICP-OES). The same applies to the results for the diffusion sources below.

[0099] The raw materials for each element were weighed so that the diffusion source had the approximate composition shown in Table 1, and the raw materials were melted and subjected to a single-roll rapid cooling method (melt spinning method) to obtain a ribbon or flake-shaped alloy. The obtained alloy was pulverized in an argon atmosphere using a mortar and then passed through a sieve with 425 μm openings to prepare an R-M alloy. The composition of the obtained R-M alloy is shown in Table 1.

[0100] The obtained sintered R-T-B based magnet material was cut and ground to form a cube measuring 7.4 mm x 7.4 mm x 7.4 mm. Next, the diffusion source was sprayed all over the surface of the sintered R-T-B based magnet material in the amount of diffusion source coating shown in Table 1. The diffusion process involved a first heat treatment in reduced pressure argon controlled to 50 Pa at the diffusion treatment temperature shown in Table 1 for 4 hours, followed by cooling to room temperature. The R-T-B based sintered magnet that had undergone the first heat treatment was then subjected to a second heat treatment in reduced pressure argon controlled to 50 Pa at 500°C shown in Table 2 for 1 hour, followed by cooling to room temperature, to produce an R-T-B based sintered magnet. The obtained sintered R-T-B based magnet was machined to form a sample measuring 7 mm x 7 mm x 7 mm, and the magnetic properties (H cJ The measurement results are shown in Table 1.

[0101] Although each of the Examples uses the same sintered R-T-B based magnet material as Comparative Examples 1 to 4, the manufacturing conditions for each of the Examples, such as the composition of the sintered R-T-B based magnet material, the composition of the diffusion source, the amount of the diffusion source applied, the first heat treatment, and the second heat treatment, are changed compared to the Comparative Examples.

[0102]

[0103] FIG. 8 shows the C obtained from the above examples and comparative examples. 1-3 Total frequency and H cJ Graph showing the relationship between "C 1-3 The "total frequency" is the total frequency of the three lowest classes in a frequency histogram of grain boundary widths measured from N reference points included in the two-particle grain boundary in a cross section of the R-T-B based sintered magnet that includes the orientation direction in the plane. 1-3 Total frequency and H cJ 10 is a table showing the relationship between

[0104] In addition, C in each example and comparative example 1-3 The total frequency was calculated using the method described above. The cross section measured was at a position (depth) of 0.1 mm from the surface of the RTB based sintered magnet. Five digital images were taken from each RTB based sintered magnet, for a total of 3,300 μm 2 Obtained.

[0105] As is clear from FIG. 8 and Table 2, C 1-3 When the total frequency exceeds 12%, H cJ According to the inventor's investigation, C 1-3 The total frequency is preferably 3% or more and 12% or less of the total. 1-3 A total frequency of 12% or less corresponds to the fact that, under the above-mentioned grain boundary width measurement conditions, the frequency of grain boundary widths of 0.03 μm or less in a frequency histogram is 12% or less overall. The frequency of grain boundary widths of 0.03 μm or less is preferably 3% or more and 12% or less.

[0106]

[0107] FIG. 9 shows the frequency (C3 frequency) of class C3 (grain boundary width in the range of 0.02 μm to 0.03 μm) and H cJ As is clear from FIG. 9, the lower the C3 frequency, the higher the H cJ increases, and the C3 frequency is preferably 5% or less (specifically, 0.5% or more and 5% or less).

[0108] The R-T-B based sintered magnets of the present disclosure can be used as permanent magnets in a wide variety of applications, such as voice coil motors (VCMs) for hard disk drives, motors for electric vehicles (EVs, HVs, PHVs), motors for industrial equipment, and other motors, as well as in home appliances.

Claims

1. An R-T-B based sintered magnet (R is at least one of rare earth elements, and must contain at least one of Nd and Pr, T is Fe or Fe and Co, and B is boron), comprising a plurality of R 2 T 14 A main phase consisting of B compound particles, and the plurality of R 2 T 14 and a grain boundary phase located between B compound particles and including a two-particle grain boundary and a grain boundary triple junction, wherein when a frequency histogram of grain boundary widths measured from N reference points included in the two-particle grain boundary in a cross section including in-plane the orientation direction of the R-T-B sintered magnet is determined so that the sixth class from the lowest class shows the most frequent value, the total frequency of the first, second and third classes from the lowest class is 12% or less of the total.

2. An R-T-B based sintered magnet (R is at least one of rare earth elements, and must contain at least one of Nd and Pr, T is Fe or Fe and Co, and B is boron), comprising a plurality of R 2 T 14 A main phase consisting of B compound particles, and the plurality of R 2 T 14 and a grain boundary phase located between B compound grains, the grain boundary phase including a two-particle grain boundary and a grain boundary triple junction, wherein in a frequency histogram of grain boundary widths measured from N reference points included in the two-particle grain boundary in a cross section including in-plane the orientation direction of the R-T-B based sintered magnet, the frequency of the grain boundary width being 0.03 μm or less is 12% or less overall.

3. The R-T-B based sintered magnet according to claim 1 or 2, wherein the cross section is located at a distance of 0.05 mm or more and 0.15 mm or less from the surface of the R-T-B based sintered magnet.

4. The R-T-B based sintered magnet according to claim 1 or 2, wherein the relationship [T] / 55.85>14×[B] / 10.8 is satisfied, where [T] is the composition ratio of T expressed in mass % and [B] is the composition ratio of B expressed in mass %.

5. The R-T-B based sintered magnet according to claim 1, wherein the total frequency of the first, second and third lowest classes in said frequency histogram is 10% or less of the total.

6. The R-T-B based sintered magnet according to claim 1, wherein the total frequency of the first, second and third lowest classes in said frequency histogram is equal to or greater than 3% and equal to or less than 12% of the total.

7. The R-T-B based sintered magnet according to claim 1 or 2, wherein the composition ratio of R in the R-T-B based sintered magnet is 31 mass % or less.

8. The R-T-B system sintered magnet according to claim 1 or 2, wherein the total composition ratio of Dy and Tb in the R-T-M system sintered magnet is 0.5 mass % or less (including 0 mass %).

9. The R-T-B based sintered magnet according to claim 1 or 2, which includes a portion where the R concentration gradually decreases from the magnet surface toward the magnet's interior.

10. The R-T-B based sintered magnet according to claim 1, wherein the frequency of grain boundary widths of 0.03 μm or less in the frequency histogram is 12% or less overall.

11. The R-T-B based sintered magnet according to claim 2, wherein the frequency of the grain boundary width in the range of 0.02 μm or more and 0.03 μm or less in the frequency histogram is 5% or less overall.

12. The R-T-B based sintered magnet according to claim 2, wherein the frequency of the grain boundary width in the range of 0.02 μm or more and 0.03 μm or less in the frequency histogram is between 0.5% and 5% of the total.

13. The RTB system sintered magnet according to claim 2, wherein the frequency of the grain boundary width being 0.03 μm or less in the frequency histogram is between 3% and 12%.

14. The R-T-B based sintered magnet according to claim 2, wherein, when the width of the classes in the frequency histogram is determined so that the sixth class from the lowest class represents the mode, the total frequency of the first, second and third classes from the lowest class is 12% or less of the total.

Citation Information

Patent Citations

  • Method for analyzing polycrystalline material

    JP2019015573A

  • Alloy for r-t-b-based rare earth sintered magnet, process for producing alloy for r-t-b-based rare earth sintered magnet, alloy material for r-t-b-based rare earth sintered magnet, r-t-b-based rare earth sintered magnet, process for producing r-t-b-based rare earth sintered magnet, and motor

    WO2013008756A1

  • R-fe-co-b-c permanent magnet alloy reduced in irreversible demagnetization and excellent in heat stability

    JP1992268051A

  • Rare earth magnet

    JP2014209546A

  • R-iron-boron based sintered magnet and method for manufacturing the same