Cation exchange membrane, ion exchange membrane cell, and electrodialysis device

The cation exchange membrane utilizing a metal cyano complex and binder resin addresses the inefficiencies in concentrating ammonium ions by ensuring high selectivity and energy efficiency, preventing scale formation and membrane damage.

WO2024203446A1PCT designated stage expired Publication Date: 2024-10-03YAMAGUCHI UNIV +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010205
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-15
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current ion exchange and electrodialysis methods face challenges in selectively concentrating specific cations like ammonium ions efficiently, leading to energy inefficiencies and membrane damage due to scale formation from divalent cations like calcium ions.

Method used

A cation exchange membrane is developed using a metal cyano complex and a binder resin with specific ratios and properties, allowing for high selectivity and permeability of ammonium ions while maintaining low energy consumption and preventing scale formation.

Benefits of technology

The membrane achieves selective concentration of ammonium ions with improved energy efficiency and reduced membrane damage, enhancing the separation and recovery of target ions in electrodialysis processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010205_03102024_PF_FP_ABST
    Figure JP2024010205_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a cation exchange membrane having high selectivity for a specific cation, particularly an ammonium ion, and also having high energy efficiency in dialysis. The cation exchange membrane has a cation exchange layer containing a metal cyano complex and a binder resin.
Need to check novelty before this filing date? Find Prior Art

Description

Cation exchange membrane, ion exchange membrane cell and electrodialysis device

[0001] The present invention relates to a cation exchange membrane, an ion exchange membrane cell and an electrodialysis apparatus using the same, and a method for producing the cation exchange membrane.

[0002] Technologies for concentrating and separating ions in wastewater include distillation, ion exchange, adsorption, reverse osmosis (RO), forward osmosis (FO), brine concentration (BC), electrodialysis (ED), and Donnan dialysis. Among these, distillation can handle a wide range of salt concentrations and water qualities and has excellent contamination resistance, but requires significant energy consumption and is particularly unsuitable for treating dilute solutions. Various ion exchangers and adsorbents have been developed for ion exchange and adsorption (see, for example, Patent Documents 1 and 2). However, continuous operation is difficult due to the need for regeneration processes for the ion exchange material and adsorbent (see Patent Documents 3 and 4). Furthermore, continuous treatment is unsuitable due to the need for equipment and chemicals for regenerating the ion exchange material and adsorbent. In the RO membrane method, ions are concentrated by applying pressure greater than the osmotic pressure to the wastewater to dehydrate it, resulting in high power costs when concentrating from dilute solutions. Furthermore, membrane cleaning and replacement are required more frequently when wastewater contains membrane foulants. Furthermore, due to the membrane's pressure limit, it is difficult to concentrate high salt concentrations. The FO membrane method, like the RO membrane method, concentrates ions by dehydration. The use of a driving force solute (DS) has the advantage of not requiring pressure or electricity, but otherwise suffers from the same problems as the RO membrane method. The brine concentration (BC) method allows for concentration of higher salt concentrations than the RO membrane method by connecting FO membrane modules in series in multiple stages, but requires a larger membrane area than the RO membrane method because a portion of the concentrated solution is refluxed. The Donnan dialysis method, like the FO membrane method, uses DS to concentrate and separate ions, so does not require electricity, but it does require separation of the DS and the target ions. While each method has its advantages and disadvantages as described above, actual treated water contains not only impurities but also various ions, and with the exception of ion exchange methods, these methods have the problems of scale formation due to these ions and reduced energy efficiency for concentrating the desired ions.

[0003] The ED method is a technology for concentrating and desalination ions using ion exchange membranes. In the concentration process, ions are transported and concentrated, making it particularly effective for separating and concentrating membrane foulants and specific trace ions. While high-concentration salt treatment requires power, this technology, like the BC method, allows for high-concentration treatment. However, the ED method also concentrates ions other than the target ion. In this case, the concentration of divalent cations such as calcium ions can lead to the formation of scale within the membrane, on the membrane surface, or within the solution flow path, resulting in membrane breakdown and reduced system efficiency (see Non-Patent Document 1). Furthermore, when targeting cations with the same valence as the target ion, such as ammonium ions, the presence of monovalent ions such as Na ions and K ions consumes power to concentrate the ion, resulting in reduced energy efficiency for separating and concentrating the target ion. Therefore, the development of an ion exchange membrane that selectively transmits specific target ions, such as ammonium ions, has been desired.

[0004] Among cations, the separation and concentration of ammonium ions in particular has attracted attention for the following reasons. Currently, nitrogen compounds in waste gases and wastewater are detoxified using a great deal of energy. However, there are cases where nitrogen compounds are released without treatment or where treatment is insufficient, resulting in significant environmental impact. Therefore, there is a need for the development of a resource ammonification technology for nitrogen compounds in wastewater that will detoxify and recycle these harmful nitrogen compounds resulting from human activities (Clean Earth). Therefore, focusing on nitrogen compounds in wastewater, development is being conducted on technologies that convert them into ammonia (including ammonium ions) and concentrate them to produce a form that can be used as a valuable resource (resource ammonia). Among these technologies, energy-saving separation and concentration of ammonium ions present in wastewater has attracted attention.

[0005] International Publication WO2015 / 186819 Pamphlet Japanese Patent Application Laid-Open No. 2012-250904 Japanese Patent Application Laid-Open No. 2019-34273 International Publication WO2020 / 080302 Pamphlet

[0006] "Selective permeability of ions in ion exchange membranes," Asahi Glass Research Report 64 (2014), pp. 21-25

[0007] An object of the present invention is to provide a cation exchange membrane which has high selectivity for specific cations, particularly ammonium ions, and which also has high energy efficiency during dialysis.

[0008] The present inventors began investigating ion exchange membranes with high selectivity for specific ions, and progressed with the development of ion exchange membranes with high permselectivity for ammonium ions, a specific target ion. During this investigation, they unexpectedly discovered that a membrane fabricated by mixing particles of metal cyano complexes (Patent Documents 1 and 2), known as adsorbents for ammonium and cesium ions, with a binder resulted in a cation exchange membrane with high permselectivity for ammonium ions. Adsorbents are primarily used in batch processes because they adsorb and retain target ions within the adsorbent. On the other hand, ion exchange membranes selectively and continuously transport only the target ions through the membrane using driving forces such as electrical and diffusive forces. Furthermore, while adsorbents are used in particulate form, ion exchange membranes can only fulfill their function when formed into thin films. For these reasons, the creation of cation exchange membranes using metal cyano complex adsorbents was previously unthinkable. This is how the present invention was completed.

[0009] That is, the present invention is characterized by the following features: (1) A cation exchange membrane having a cation exchange layer containing a metal cyano complex and a binder resin. (2) The cation exchange membrane according to (1) above, in which the mass ratio of the metal cyano complex to the binder resin is 0.2:1 to 5:1. (3) A membrane resistance of 0.2 to 15 Ωcm. 2(4) The cation exchange membrane according to any one of (1) to (3) above, wherein the binder resin is a resin having no ion exchange capacity and / or a resin having low ion exchange capacity. (5) The cation exchange membrane according to (4) above, wherein the resin having low ion exchange capacity has an ion exchange capacity of 0.001 to 0.2 meq / g. (6) The cation exchange membrane according to any one of (1) to (5) above, wherein a cation exchange layer containing a metal cyano complex and a binder resin is provided on one or both sides with another cation exchange layer not containing a metal cyano complex. (7) An ion exchange membrane cell in which an anion exchange membrane and the cation exchange membrane according to any one of (1) to (6) above are arranged opposite each other. (8) An electrodialysis apparatus comprising an anode, a cathode, a cation exchange membrane, and an anion exchange membrane, wherein the cation exchange membrane is the cation exchange membrane according to any one of (1) to (6) above. (9) A method for producing a cation exchange membrane, comprising mixing metal cyano complex particles, a binder resin, and a solvent, dispersing the metal cyano complex particles in the mixed solution, and applying or casting the mixed solution to remove the solvent. (10) A method for producing a cation exchange membrane, comprising mixing metal cyano complex particles, a binder resin, and a solvent, dispersing the metal cyano complex particles in the mixed solution, and applying or casting the mixed solution to remove the solvent, and then applying a mixture of a resin and a solvent to form another cation exchange layer that does not contain a metal cyano complex to the resulting cation exchange layer, and then removing the solvent, or adhering another cation exchange membrane that does not contain a metal cyano complex. The present invention is further characterized by the following: (i) A cation exchange membrane having a cation exchange layer containing a metal cyano complex and a binder resin. (ii) The cation exchange membrane of (ii) above, having another cation exchange layer on one or both sides of the cation exchange layer containing a metal cyano complex and a binder resin. (iii) The cation exchange membrane of (i) or (ii) above, in which the binder resin is a resin having no ion exchange capacity and / or a resin having low ion exchange capacity. (iv) An ion exchange membrane cell in which an anion exchange membrane and the cation exchange membrane of (i) or (ii) above are arranged facing each other. (v) An electrodialysis apparatus comprising an anode, a cathode, a cation exchange membrane, and an anion exchange membrane, wherein the cation exchange membrane is the cation exchange membrane of (i) or (ii) above.

[0010] The cation exchange membrane of the present invention has excellent selective permeability to specific cations, particularly ammonium ions. The ion exchange membrane cell of the present invention can be used in devices such as electrodialysis to selectively concentrate specific cations, particularly ammonium ions. The electrodialysis device of the present invention can selectively concentrate specific cations, particularly ammonium ions. The cation exchange membrane, ion exchange membrane cell, and electrodialysis device of the present invention can improve energy efficiency during dialysis.

[0011] FIG. 1 is a schematic diagram showing an example of using an ion exchange membrane cell of the present invention. FIG. 2 is a scanning electron microscope (SEM) image of the pulverized metal cyano complex used in Example 1. FIG. 3 is a scanning electron microscope (SEM) image of the pulverized metal cyano complex used in Example 2. FIG. 4 is a scanning electron microscope (SEM) image of the membrane produced in Example 2. FIG. 5 is a scanning electron microscope (SEM) image of the membrane produced in Example 3. FIG. 6 is a scanning electron microscope (SEM) image of the membrane produced in Example 4. FIG. 7 is a diagram showing the measuring device and measurement conditions for membrane resistance used in Examples and Comparative Examples. FIG. 8 is a diagram showing the electrodialysis test device used in Examples and Comparative Examples. FIG. 9 is a diagram showing the electrodialysis test results for Example 1. FIG. 10 is a diagram showing the electrodialysis test results for Example 2. FIG. 11 is a diagram showing the electrodialysis test results for Example 3. FIG. 12 is a diagram showing the electrodialysis test results for Example 4. FIG. 13 is a diagram showing the electrodialysis test results for Example 5. Fig. 14 is a diagram showing the results of the electrodialysis test of Example 9. Fig. 15 is a diagram showing the results of the electrodialysis test of the comparative example.

[0012] The cation exchange membrane of the present invention is a cation exchange membrane having a cation exchange layer containing a metal cyano complex having cation exchange ability and a binder resin. The metal cyano complex in the present invention is not particularly limited, but for example, its composition is x M [M' (CN) 6 ] y ・zH 2Here, the metal atom M is preferably one or more metal atoms selected from the group consisting of vanadium, chromium, manganese, iron, ruthenium, cobalt, rhodium, nickel, palladium, platinum, copper, silver, zinc, lanthanum, europium, gadolinium, lutetium, barium, strontium, and calcium, more preferably one or more metal atoms selected from the group consisting of vanadium, chromium, manganese, iron, ruthenium, cobalt, nickel, copper, and zinc, and particularly preferably one or more metal atoms selected from the group consisting of manganese, iron, cobalt, nickel, copper, and zinc. The metal atom M' is preferably one or more metal atoms selected from the group consisting of vanadium, chromium, molybdenum, tungsten, manganese, iron, ruthenium, cobalt, nickel, platinum, and copper, more preferably one or more metal atoms selected from the group consisting of manganese, iron, ruthenium, cobalt, and platinum, and more preferably one or more metal atoms selected from the group consisting of iron and cobalt. A is a monovalent or more polyvalent cation, preferably one or more cations selected from the group consisting of hydrogen, ammonium, alkali metals, and alkaline earth metals, and more preferably one or more cations selected from the group consisting of hydrogen, lithium, sodium, potassium, rubidium, and cesium.

[0013] Furthermore, when M and M' are identified, it is called an M-M' cyano complex. For example, when M=copper and M'=iron, it is called a copper-iron cyano complex. x is preferably 0 to 3, more preferably 0 to 2.5, and even more preferably 0 to 2. y is preferably 0.1 to 1.5, more preferably 0.4 to 1.3, and even more preferably 0.5 to 1. z is preferably 0 to 6, more preferably 0.5 to 5.5, and even more preferably 1 to 5. The crystal structure of a metal cyano complex is generally a face-centered cubic structure, but is not necessarily limited to this. For example, K 0.67 Zn[Fe(CN)6] 0.67-zHO forms a hexagonal crystal. Furthermore, while six cyano groups are typically coordinated to M', some of these may be substituted with nitro groups, etc., and there is no problem if the number is within four to eight. There are no particular limitations on the synthesis method for metal cyano complexes, but a method that can uniformly achieve the desired composition is preferred. For processing convenience, the complex surface may be modified with various materials. Specific methods include those described in, for example, JP 2006-256954 A and JP 2013-173077 A, and nanoparticles with a large specific surface area are desirable. Furthermore, since uniform particles are desirable for practical use, the uniform nanoparticle production method described in JP 2013-173077 A is appropriate. Metal cyano complexes are provided as powders or slurries dispersed in water, but the form is not limited to these. As described below, it is important that the metal cyano complex and the binder resin are mixed uniformly, so it is desirable to select an appropriate combination of the form of the metal cyano complex and the binder. As described in Japanese Patent No. 5035767 and Japanese Patent Publication No. 2008 / 081923, the dispersibility of the metal cyano complex in various solvents can be controlled by adding metal ions, ferrocyanide ions, organic molecules, or the like to the particle surface. When using a binder that disperses in water, it is desirable to improve the dispersibility of the metal cyano complex in water. When using a binder that disperses or dissolves in an organic solvent, it is desirable to improve the dispersibility of the metal cyano complex in the organic solvent.

[0014] The binder resin in the present invention is not particularly limited as long as it can fix the metal cyano complex particles to form a layer or film containing the metal cyano complex particles. The binder resin in the present invention is preferably one that has excellent dispersibility of the metal cyano complex particles, i.e., one that uniformly disperses the complex particles without uneven distribution within the resin. From the viewpoint of ease of mixing with the metal cyano complex particles, one that is plastic, particularly thermoplastic, is preferred. From the same viewpoint of ease of mixing with the metal cyano complex particles, one that is dispersible in water or dispersible or soluble in organic solvents can be used, but one that is soluble in a general-purpose organic solvent is preferred. In the present invention, a plastic binder resin is one that has the property of being deformed by the application of an external force and not returning to its original shape even when the force is removed (if a support, as described below, is used, it is one that has this property together with the support). It includes polymers that are plastic at room temperature and polymers that have thermoplasticity, which soften when heated to make them easier to mold and then harden again when cooled.

[0015] The binder resin in the present invention is preferably one that has no ion exchange capacity or one that has a low ion exchange capacity that is lower than that of conventional ion exchange membranes. In the present invention, a binder resin having a low ion exchange capacity refers to one that has an ion exchange group but has a smaller ion exchange capacity than that of conventional ion exchange membranes. Examples of the ion exchange group include -CF 2 SO 3 H, -SO 3 H, -CF 2 COOH, -COOH, -PO 3 H 2 , -Phenolic OH, -C(CF 3 ) 3 OH, -CF 2 SO 2 Cation exchange groups (anionic groups) such as NHR, -N(CH 3 ) 3 OH, -N(CH 2 OH)(CH 3 ) 2 OH, -S(CH 3 ) 2 OH, -P(CH 3 ) 3OH、-NH 2 、-NH、Aniline(NH 2Examples of the binder resin having low ion exchange capacity include anion exchange groups (cationic groups) such as ethylene glycol fluoride (e.g., propylene glycol fluoride), propylene ... Specific examples include polymers of aliphatic olefins such as the aforementioned polyethylene, polypropylene, polybutylene, and polybutadiene; polymers of aromatic olefins such as polystyrene, poly-α-methylstyrene, and polydivinylbenzene; polymers of oxygen-containing olefins such as polymethyl methacrylate, polyvinyl acetate, and the aforementioned polyvinyl alcohol; polymers of nitrogen-containing olefins such as the aforementioned polyacrylonitrile and poly-N-methylpyrrolidone; polymers of halogen-containing olefins such as polyvinyl chloride, polyvinylidene chloride, and the aforementioned polyvinylidene fluoride and polytetrafluoroethylene. These polyolefins may be used alone or in combination. Copolymers or graft copolymers of two or more of the above-mentioned olefins may also be used. Other examples include polyether ketone, polyether ether ketone, polyphenylene, polyphenylene oxide, polyphenylene ether, modified polyphenylene ether, polyphenylene sulfide, and polyetherimide. In the present invention, one binder resin or two or more binder resins may be used. When a binder resin having cation exchange capacity is used in the present invention, if other cations as well as specific cations such as ammonium ions permeate through the binder resin portion, the effect of the present invention, that is, excellent selective permeability for ammonium ions, may be reduced. When a binder resin having anion exchange capacity is used, there is a risk that anions may also be permeated through the binder resin portion.Therefore, when using a binder resin having an ion exchange group in the present invention, it is preferable that the ion exchange capacity be within the above range, which results in low ion exchange capacity, whether the binder resin has a cation exchange group or an anion exchange group.

[0016] When using a binder resin having an ion exchange group in the present invention, a cationic or anionic ion exchange group may be introduced into a binder resin such as a nonionic polymer that does not have an ion exchange group, or a cationic or anionic polymer may be mixed with a binder resin such as a nonionic polymer that does not have an ion exchange group. A cationic polymer is a polymer that contains a cationic group (positively charged group) in the molecular chain, and the cationic group may be contained in the main chain, side chain, or terminal. Examples of cationic groups in cationic polymers include ammonium groups, iminium groups, sulfonium groups, and phosphonium groups, as well as the cationic groups described above. Polymers containing functional groups, such as amino groups and imino groups, a portion of which can be converted to ammonium groups or iminium groups in water, are also included in the cationic polymer of the present invention. Among these, ammonium groups are preferred from the viewpoint of industrial availability. The ammonium group may be a primary ammonium group (ammonium group), a secondary ammonium group (e.g., alkylammonium group), a tertiary ammonium group (e.g., dialkylammonium group), or a quaternary ammonium group (e.g., trialkylammonium group), with a quaternary ammonium group (e.g., trialkylammonium group) being more preferred. The cationic polymer may contain only one type of cationic group, or may contain multiple types of cationic groups. The counter anion of the cationic group is not particularly limited, and examples include halide ions, hydroxide ions, phosphate ions, and carboxylate ions. Among these, halide ions are preferred, and chloride ions are more preferred, from the viewpoint of ease of availability. The cationic polymer may contain only one type of counter anion, or may contain multiple types of counter anions. The cationic polymer used in the present invention may be a polymer consisting solely of structural units containing cationic groups, or may be a polymer consisting of both structural units containing cationic groups and structural units not containing cationic groups. These polymers may also be crosslinkable. The cationic polymer may be composed of only one type of polymer, or may contain multiple types of polymers.Furthermore, the polymer may be a mixture of a polymer containing a cationic group and a polymer not containing a cationic group.

[0017] An anionic polymer is a polymer containing an anionic group (negatively charged group) in the molecular chain, and the anionic group may be contained in any of the main chain, side chain, and terminal. Examples of the anionic group in an anionic polymer include sulfonate groups, carboxylate groups, phosphonate groups, and the like, as well as the aforementioned anionic groups. Furthermore, polymers containing functional groups, such as sulfonic acid groups, carboxyl groups, and phosphonic acid groups, a portion of which can be converted to sulfonate groups, carboxylate groups, or phosphonate groups in water, are also included in the anionic polymer of the present invention. Among these, sulfonate groups are preferred due to their large ionic dissociation constant. Anionic polymers may contain only one type of anionic group, or may contain multiple types of anionic groups. Furthermore, the counter anion of the anionic group is not particularly limited, and examples include hydrogen ions and alkali metal ions. Among these, alkali metal ions are preferred due to their reduced corrosion potential. The anionic polymer may contain only one type of counter cation, or may contain multiple types of counter cations. The anionic polymer used in the present invention may be a polymer consisting only of structural units containing an anionic group, or may be a polymer consisting of both structural units containing an anionic group and structural units not containing an anionic group. Furthermore, these polymers may be crosslinkable. The anionic polymer may be composed of only one type of polymer, or may contain multiple types of polymers. Furthermore, it may be a mixture of a polymer containing an anionic group and a polymer not containing an anionic group.

[0018] Furthermore, the cation exchange layer of the present invention containing a metal cyano complex and a binder resin (hereinafter also referred to as the "cation exchange layer of the present invention") may contain a third component other than the binder resin to improve the dispersibility of the metal cyano complex in the binder resin. In the present invention, even if permeation of unintended ions occurs, the addition of a third component to the binder resin is not prohibited, as improving the dispersibility of the metal cyano complex takes priority. This third component is mixed with the binder resin, unlike a direct surface treatment of the metal cyano complex particles themselves. Examples of the third component include the nonionic polymers, cationic polymers, and anionic polymers described above.

[0019] The cation exchange layer of the present invention containing a metal cyano complex and a binder resin is a cation exchange layer in which metal cyano complex particles are dispersed in the binder resin. The cation exchange layer of the present invention is not particularly limited as long as it is a layer in which the metal cyano complex particles are fixed by the binder resin. For example, the metal cyano complex particles may be fixed by embedding all or part of the surface of the metal cyano complex particles in the binder resin, or the metal cyano complex particles may be fixed by filling the spaces between the metal cyano complex particles with the binder resin. The cation exchange layer of the present invention may consist solely of a metal cyano complex and a binder resin, or may contain components other than the metal cyano complex and the binder resin. Furthermore, the cation exchange membrane of the present invention may consist solely of a cation exchange layer containing a metal cyano complex and a binder resin, or may contain, in addition to the cation exchange layer containing a metal cyano complex and a binder resin, other cation exchange layers, supports, etc., as described below. When the cation exchange membrane of the present invention is composed solely of a cation exchange layer containing a metal cyano complex and a binder resin, the cation exchange layer containing the metal cyano complex and the binder resin is in a membranous form, and the cation exchange membrane of the present invention is a cation exchange membrane containing a metal cyano complex and a binder resin. The cation exchange layer or membrane containing the metal cyano complex and the binder resin has excellent selective permeability for ammonium ions.

[0020] The ratio of the content of the metal cyano complex to the binder resin in the cation exchange layer containing the metal cyano complex and the binder resin in the present invention is not particularly limited, but the mass ratio of the metal cyano complex to the binder resin is preferably 0.2:1 to 5:1, preferably 0.5:1 to 3:1, more preferably 0.75:1 to 2:1, and even more preferably 0.9:1 to 1.8:1. That is, the mass ratio of the metal cyano complex to 1 mass of the binder resin is preferably 0.2 to 5, preferably 0.5 to 3, more preferably 0.75 to 2, and even more preferably 0.9 to 1.8. If the content of the metal cyano complex is less than the lower limit of the preferred mass ratio range, the membrane resistance may be increased and the selective permeability of monovalent cations, particularly ammonium ions, may be reduced. On the other hand, if the content of the metal cyano complex is greater than the upper limit of the preferred mass ratio range, the mechanical strength of the membrane may be reduced, and the selective permeability of ammonium ions, in particular, may be reduced.

[0021] The particle size of the metal cyano complex particles contained in the cation exchange layer in the present invention is not particularly limited, but the crystallite size, as evaluated using X-ray structural diffraction and Scherrer's law from the line width of the X-ray pattern, is preferably 2 μm or less, more preferably 0.005 to 0.5 μm. In the cation exchange layer, the metal cyano complex may exist as primary particles of crystallite size, primary particles formed by bonding multiple crystallites, or secondary particles formed by agglomeration of primary particles due to intermolecular forces, etc. When present as primary particles in the cation exchange layer, the primary particle size is preferably 5 μm or less, more preferably 2 μm or less. Furthermore, the primary particle size in the cation exchange layer is preferably 0.005 to 1.0 μm, and the secondary particle size is preferably 0.1 to 5 μm. The primary particle size and secondary particle size in the cation exchange layer can be determined by observation with a scanning electron microscope (SEM). The shapes of primary particles and secondary particles include irregular, approximately elliptical, approximately spherical, etc., and here, the maximum length of a straight line drawn between two points on the outer edge of a particle in an SEM image is referred to as the primary particle diameter or secondary particle diameter. Here, the preferred range means that 90% or more, more preferably 95% or more of the number of metal cyano complex particles in the cation exchange layer are within this range. For example, "preferably 5 μm or less" means that 90% or more, more preferably 95% or more of the number of metal cyano complex particles are 5 μm or less. If the primary particle diameter or secondary particle diameter exceeds 5 μm, the area through which cations pass becomes narrow, which may increase the membrane resistance. Furthermore, unevenness may form on the membrane surface, which may lead to membrane rupture and other mechanical strength reductions. Furthermore, if the primary particle diameter or secondary particle diameter is larger than 5 μm, the amount of binder resin adhering to the particles may become sparse, resulting in the formation of one or more gaps where neither particles nor resin are present, and there is also a risk that cations may short-pass through these gaps.

[0022] The thickness of the cation exchange layer containing a metal cyano complex and a binder resin in the present invention is not particularly limited, but is preferably 5 to 300 μm, more preferably 10 to 100 μm. If the thickness of the cation exchange layer is too thin, the mechanical strength may decrease, and if the thickness is too thick, the electrical resistance may increase. Furthermore, the cation exchange membrane of the present invention, or the cation exchange layer when the cation exchange membrane of the present invention is composed only of a cation exchange layer containing a metal cyano complex and a binder resin, has a membrane resistance, which represents electrical resistance, of 0.2 to 15 Ω cm. 2 is preferably 0.3 to 10 Ωcm 2 More preferably, 0.5 to 5 Ωcm 2 is more preferable.

[0023] In a cation exchange layer containing a metal cyano complex and a binder resin, specific cations are separated and concentrated by selectively migrating through the metal cyano complex particles and permeating out of the layer. Therefore, it is desirable for the metal cyano complex particles to be uniformly dispersed within the layer. In a uniformly dispersed state, as described above, the metal cyano complex particles are contained in the cation exchange layer at a predetermined mass ratio relative to the binder resin, i.e., at a predetermined content within the cation exchange layer. Adjacent particles contact each other, and cations can pass through the layer, migrating through the particles like a string of beads, through these contact points. This is a different particle existence condition from when target ions are adsorbed onto particles in a liquid. While a certain content within the cation exchange layer is necessary, if the content is too high throughout the layer or in part of the layer, the binder resin adhering to the particles may become sparse, resulting in one or more gaps, as in the case where the primary or secondary particle size of the metal cyano complex exceeds a predetermined size. If cations other than those intended for concentration and separation pass through the gaps created in the cation exchange layer in a short-path manner, separation and recovery of the intended cations will be hindered. Furthermore, if anions pass through the gaps in the opposite direction to the cations, this may result in a decrease in energy efficiency, such as current efficiency. Furthermore, there is a concern that the mechanical strength of the cation exchange layer may also be reduced. Therefore, it may be necessary to provide another cation exchange layer, as described below, on the cation exchange layer containing a metal cyano complex and a binder resin.

[0024] The cation exchange membrane of the present invention may have another cation exchange layer on one or both sides of the cation exchange layer containing a metal cyano complex and a binder resin. Hereinafter, the term "another cation exchange layer" refers to a cation exchange layer other than the one containing a metal cyano complex and a binder resin. The other cation exchange layer is preferably a cation exchange layer that does not contain a metal cyano complex, and more preferably a cation exchange layer with a cation ion exchange capacity of more than 0.2 meq / g. Furthermore, the other cation exchange layer is preferably free of a metal cyano complex and a binder resin. Here, "free of a metal cyano complex" and "free of a binder resin" do not exclude the inclusion of trace amounts of a metal cyano complex or a binder resin to the extent that the function of the other cation exchange layer in the present invention is not impaired. In a cation exchange layer containing a metal cyano complex and a binder resin, cations and / or anions may migrate through the gaps formed as described above, which may make it difficult to separate and collect the target cations or reduce the current efficiency. In this case, anions move in the opposite direction to cations within the cation exchange layer of the present invention. Therefore, by forming another cation exchange layer, permeation of cations and anions within the gaps can be prevented, facilitating the separation and recovery of the target cations and preventing a decrease in current efficiency. Furthermore, by forming another cation exchange layer, the mechanical strength of the ion exchange membrane can be improved. The material of the other cation exchange layer is not particularly limited, and any material that can be used as a cation exchange membrane can be used. However, materials with high bonding strength with the binder resin are preferred, as well as materials with low membrane resistance and high mechanical strength. Examples of materials constituting the other cation exchange layer include sulfonated polyethersulfone and polyvinyl alcohol copolymers. Examples of polyvinyl alcohol copolymers include PVA-b-PSS and PVA-b-VBTAC, as described in WO 2016 / 133170. Furthermore, examples of the anionic polymers described above for cation exchange layers containing a metal cyano complex and a binder resin can be used. Alternatively, a mixture of a resin having no ion exchange capacity and a resin having ion exchange capacity, such as polyethersulfone and sulfonated polyethersulfone, may be used.A resin having ion exchange capacity may be used as a base material of a resin having no ion exchange capacity. For example, a nonionic polymer in a cation exchange layer containing a metal cyano complex and a binder resin can be used as the resin having no ion exchange capacity. Similarly, the ion exchange group (anionic group) described above can be used as the ion exchange group for imparting ion exchange capacity. Another example of a cation exchange layer in the present invention is a cation exchange layer formed from an anionic polymer.

[0025] The thickness of the other cation exchange layer is not particularly limited, but is preferably 1 to 100 μm, more preferably 2 to 50 μm. If the thickness of the other cation exchange layer is too thin, the mechanical strength may decrease, and if the thickness is too thick, the membrane resistance may become too high. The ratio of the thickness of the cation exchange layer containing a metal cyano complex and a binder resin to the thickness of the other cation exchange layer (if the other cation exchange layer is present on both sides, the total thickness of both sides; the same applies hereinafter) is preferably 1:0.1 to 1:100, more preferably 1:0.3 to 1:50, and even more preferably 1:0.5 to 1:10. That is, when the thickness of the cation exchange layer containing a metal cyano complex and a binder resin is taken as 1, the ratio of the thickness of the other cation exchange layer to the thickness of the cation exchange layer is preferably 0.1 to 100, more preferably 0.3 to 50, and even more preferably 0.5 to 10.

[0026] The thickness of the cation exchange membrane in which another cation exchange layer is provided on one or both sides of the cation exchange layer containing a metal cyano complex and a binder resin is not particularly limited, but is preferably 10 to 400 μm, more preferably 20 to 200 μm, and even more preferably 25 to 120 μm. The membrane resistance of the cation exchange membrane in which another cation exchange layer is provided is preferably 0.5 to 10 Ωcm. 2 , 0.7 to 5 Ωcm 2 is preferred.

[0027] The cation exchange membrane of the present invention may have a support. The presence of a support improves mechanical strength. The support may be present in the cation exchange layer containing a metal cyano complex and a binder resin, or in another cation exchange layer if another cation exchange layer is present, or may be present on one or both sides of the cation exchange membrane of the present invention. The support is not particularly limited as long as it has openings, and examples thereof include mesh, nonwoven fabric, woven fabric, various porous membranes, etc.

[0028] The method for producing the ion exchange membrane of the present invention is not particularly limited, but examples include a method in which metal cyano complex particles, a binder resin, and a solvent are mixed, the metal cyano complex particles are thoroughly dispersed in the mixed solution, and the mixed solution is applied, cast, or the like, to remove the solvent to form a membrane. Methods for forming the other cation exchange layer are not particularly limited, but examples include a method in which a resin forming the other cation exchange layer is mixed with a solvent, applied to a cation exchange layer containing a metal cyano complex and a binder resin, and the solvent is removed, and a method in which a cation exchange membrane forming the other cation exchange layer is bonded to a cation exchange layer containing a metal cyano complex and a binder resin. The metal cyano complex particles used in producing the cation exchange membrane of the present invention preferably have a crystallite size of 2 μm or less, preferably 0.005 to 0.5 μm, as evaluated using X-ray structural diffraction from the line width of the X-ray pattern using Scherrer's law. The metal cyano complex particles used may exist as primary particles of crystallite size, primary particles formed by bonding multiple crystallites, or secondary particles formed by agglomeration of primary particles due to intermolecular forces, etc. When present as primary particles, the primary particle diameter is preferably 5 μm or less, and when present as secondary particles, the secondary particle diameter is preferably 2 μm or less. Furthermore, the primary particle diameter of the metal cyano complex particles used is preferably 0.005 to 1.0 μm, and the secondary particle diameter is preferably 0.1 to 5 μm. The primary particle diameter and secondary particle diameter can be determined using a scanning electron microscope in the same manner as described in paragraph

[0021] above. It is preferable to uniformly disperse the metal cyano complex particles in the binder resin so that the primary particle diameter and secondary particle diameter of the metal cyano complex particles in the produced cation exchange layer fall within the preferred particle diameter ranges for the cation exchange layer described above. When a support is used, a mixed solution of metal cyano complex particles, a binder resin, and a solvent is applied to a support such as a mesh, nonwoven fabric, woven fabric, or porous membrane, and the mixed solution is impregnated into the support or the support is immersed in the mixed solution, followed by removing the solvent to produce a cation exchange membrane having a support. The solvent is not particularly limited, but is preferably one in which the binder resin is easily dispersed or dissolved and the metal cyano complex particles are easily dispersed.Examples of the solvent include hydrocarbons such as benzene, xylene, toluene, and hexane; alcohols such as methanol, ethanol, and isopropyl alcohol; ketones such as acetone, methyl isopropyl ketone, and cyclohexane; ethers such as dioxane and tetrahydrofuran; esters such as ethyl acetate and butyl acetate; and nitrogen-containing compounds such as isopropylamine, diethanolamine, N-methylformamide, N,N-dimethylformamide, and dimethyl sulfoxide. At least one of these can be selected and used as appropriate.

[0029] In the ion exchange membrane cell of the present invention, an anion exchange membrane and a cation exchange membrane of the present invention are arranged facing each other. The anion exchange membrane in the ion exchange membrane cell of the present invention is not particularly limited as long as it is a membrane that selectively permeates anions. Figure 1 shows an example of the use of the ion exchange membrane cell of the present invention, in which ion exchange membrane cells of the present invention are stacked for use in an electrodialysis device. When another cation exchange layer is provided on one side, it is preferable to have the cation exchange layer containing a metal cyano complex and a binder resin facing the anode. In the electrodialysis device of Figure 1, a dilute side solution is passed through the anode side of the cation exchange membrane of the present invention, and a concentrate side solution is passed through the cathode side. A solution containing various ions is introduced into the dilute side, and as the introduced solution passes between the anion exchange membrane and the cation exchange membrane of the present invention, specific cations in the solution, such as ammonium ions, selectively permeate the cation exchange membrane of the present invention and move to the concentrate side. Thus, ammonium ions are concentrated in the concentrate side. Various ions may be present in the dilute side solution, and the selectivity of the cation exchange membrane of the present invention allows specific cations to be selectively concentrated. The various cations present in the dilute solution are not particularly limited, but include, for example, alkali metal ions, alkaline earth metal ions, and other monovalent to trivalent cations, such as ammonium ions, sodium ions, potassium ions, lithium ions, calcium ions, magnesium ions, and hydrogen ions, as well as heavy metal ions such as silver ions, copper ions, zinc, and mercury. The various anions present in the dilute solution are not particularly limited, but include, for example, hydroxide ions, chloride ions, bromine ions, fluoride ions, iodide ions, carbonate ions, nitrate ions, sulfate ions, and phosphate ions. The solution introduced into the concentrate side is not particularly limited, but includes, for example, the raw water to be concentrated, water in which specific ions in the raw water have been concentrated, or water, which may contain the various ions contained in the dilute solution. Examples of water that can be used include tap water, industrial water, and pure water. In the electrodialysis apparatus shown in FIG. 1 , illustrations of mesh-equipped gaskets disposed between the ion exchange membranes, power supplies for supplying power to the anode and cathode, piping for supplying solutions to the dilution side and concentration side, pumps, etc. are omitted.For example, those generally used in electrodialysis devices can be used.

[0030] In the cation exchange membrane and electrodialysis apparatus of the present invention, when another cation exchange layer is provided on one side, by orienting the cation exchange layer containing a metal cyano complex and a binder resin toward the anode, i.e., by orienting the other cation exchange layer toward the cathode, the effect of preventing anion migration from the cathode to the anode can be further improved, thereby increasing current efficiency. Conversely, when the cation exchange layer containing a metal cyano complex and a binder resin is orientated toward the cathode, i.e., when the other cation exchange layer is orientated toward the anode, if the specific cation is ammonium ion, cations other than ammonium ion may also be distributed in high concentrations in the other cation exchange layer, which may reduce ammonium ion selectivity and may reduce anion blocking ability compared to when the other cation exchange layer is orientated toward the cathode. The above description has been given of providing another cation exchange layer on one or both sides of a cation exchange layer containing a metal cyano complex and a binder resin. However, providing another cation exchange layer can be applied not only to a cation exchange layer containing a metal cyano complex and a binder resin, but also to a cation exchange layer containing an inorganic cation exchanger and a binder resin. In this case, the other cation exchange layer refers to a cation exchange layer other than a cation exchange layer containing an inorganic cation exchanger and a binder resin. Examples of inorganic ion exchangers include, but are not limited to, tantalum antimonate, zirconium phosphate, polyantimonic acid, and crystalline antimonic acid. However, in the cation exchange membrane of the present invention having another cation exchange layer on one or both sides of a cation exchange layer containing an inorganic ion exchanger and a binder resin, zeolites are excluded because they are difficult to use for the direct purpose of ion exchange and their crushed particles tend to aggregate. In the cation exchange membrane of the present invention having another cation exchange layer on one or both sides of a cation exchange layer containing an inorganic cation exchanger and a binder resin, the binder resin and other components in the cation exchange layer containing an inorganic cation exchanger and a binder resin, the raw materials, manufacturing method and manufacturing conditions for the cation exchange membrane such as the other cation exchange layer, etc. are the same as those described above for the cation exchange membrane having a cation exchange layer containing a metal cyano complex and a binder resin.

[0031] The present invention will be specifically described below with reference to examples of the present invention, but the technical scope of the present invention is not limited to these examples.

[0032] The polymers, adsorbents, and ion exchange membranes used in the examples and comparative examples were prepared as follows: 1. Polyethersulfone (Sumikaexcel PES (grade: 5900P), manufactured by Sumitomo Chemical Co., Ltd., hereinafter referred to as PES) 2. Sulfonated polyethersulfone (EW0710, manufactured by Konishi Chemical Industry Co., Ltd., hereinafter referred to as SPES) 3. Metal cyano complex K 2 Cu 3 [Fe(CN) 6 ] 2 (Hereinafter, also referred to as KCuHCF) 4. Metal cyano complex K 2 Zn 3 [Fe(CN) 6 ] 2 (Hereinafter, also referred to as KZnHCF.) 5. Standard cation exchange membrane: Neosepta (registered trademark) CSE (manufactured by Astom Corporation)

[0033] (Preparation of KCuHCF) A raw material solution A prepared by dissolving 97 g of copper sulfate pentahydrate in 555 mL of water was mixed with a raw material solution B prepared by dissolving 110 g of potassium ferrocyanide trihydrate in 555 mL of water to obtain a KCuHCF slurry containing 100 g of KCuHCF (assumed to be tetrahydrate). Next, potassium sulfate, a by-product, was removed by decantation and centrifugation to obtain a washed KCuHCF slurry. 41 g of potassium ferrocyanide trihydrate was then added, and the mixture was shaken for 3 days to obtain a surface-treated KCuHCF slurry.

[0034] (Preparation of KZnHCF) A raw material solution C prepared by dissolving 0.38 mol of zinc salt in 537 mL of water was mixed with a raw material solution D prepared by dissolving 0.26 mol of potassium ferrocyanide trihydrate in 551 mL of water to obtain a KZnHCF slurry containing 100 g of KZnHCF (assumed to be tetrahydrate). Next, potassium sulfate, a by-product, was removed by decantation and centrifugation to obtain a washed KZnHCF slurry. Further, 41 g of potassium ferrocyanide trihydrate was added, and the mixture was shaken for 3 days to obtain a surface-treated KZnHCF slurry.

[0035] Example 1 The washed KCuHCF slurry was dried, and 2 g of the dried KCuHCF was placed in a mortar and crushed 4,000 times using a pestle. An image of the crushed KCuHCF particles observed with a scanning electron microscope (SEM) (Keyence VE-8800) is shown in Figure 2. The crushed KCuHCF particles formed secondary particles, and the secondary particle diameter was determined from the SEM image using the same method as in paragraph

[0021] to be 0.2 μm or less. PES was added to N,N-dimethylacetamide (DMAc) so that the PES concentration was 20% by mass, and the mixture was dissolved by stirring with a magnetic stirrer while heating to 60°C in an oil bath. The crushed KCuHCF particles were added to the previously prepared PES DMAc solution so that the mass ratio of KCuHCF to PES was 1:1, and the mixture was mixed with a magnetic stirrer for 1 hour to disperse the particles in the PES DMAc solution. The mixture was then degassed in an ultrasonic bath for 10 minutes. The resulting solution was applied to a glass plate using a film applicator (Cortic Co., Ltd., KT-3405) with the applicator set to a height of 0.3 mm, and molded into a film. The resulting mixture was then dried on a hot plate at 60°C for 1 hour to evaporate the DMAc, yielding a film containing KCuHCF (hereinafter also referred to as a KCuHCF film). The resulting film was immersed in ion-exchange water and peeled from the glass plate. The secondary particle diameter of the KCuHCF particles in the KCuHCF film was also approximately the same as the secondary particle diameter after crushing.

[0036] Example 2 The washed KZnHCF slurry was dried, and 2 g of the dried KZnHCF was placed in a mortar and crushed 4,000 times using a pestle. Figure 3 shows an image of the crushed KZnHCF particles observed with a scanning electron microscope (SEM). The crushed KZnHCF particles formed secondary particles, and the secondary particle diameter was measured in the same manner as in Example 1, and was found to be in the range of 0.5 to 1.0 μm. A membrane containing KZnHCF (hereinafter also referred to as a KZnHCF membrane) was obtained in the same manner as in Example 1, except that the metal cyano complex was changed from KCuHCF to KZnHCF. The secondary particle diameter of the KZnHCF particles in the KZnHCF membrane was also approximately the same as the secondary particle diameter after crushing. The obtained membrane was immersed in ion-exchange water and peeled from the glass plate. The cross section and surface of the prepared membrane were observed with a scanning electron microscope, and the results are shown in Figure 4. FIG. 4(a) shows the results of observing the cross section, and FIG. 4(b) shows the results of observing the film surface.

[0037] Example 3 A membrane containing KZnHCF was obtained in the same manner as in Example 2, except that the blending ratio (mass ratio) of KZnHCF to PES was set to 1.5:1. The cross section and surface of the prepared membrane were observed with a scanning electron microscope, and the results are shown in Figure 5. Figure 5(a) shows the cross section, and Figure 5(b) shows the surface.

[0038] Example 4 A membrane containing KZnHCF was obtained in the same manner as in Example 2, except that the blending ratio (mass ratio) of KZnHCF to PES, KZnHCF:PES, was set to 1.9:1. The cross section and surface of the prepared membrane were observed with a scanning electron microscope, and the results are shown in Figure 6. Figure 6(a) shows the cross section, and Figure 6(b) shows the surface.

[0039] Example 5 A solution was prepared in the same manner as in Example 2, in which the same crushed KZnHCF particles as used in Example 2 were dispersed in a PES DMAc solution. The prepared solution was applied to a glass plate and formed into a film in the same manner as in Example 2. The solution was then dried on a hot plate at 60°C for 30 minutes to evaporate a portion of the DMAc. Meanwhile, SPES was added and dissolved in DMAc so that the SPES concentration was 20% by mass. The solution in which SPES was dissolved in DMAc was dropped onto the previously dried KZnHCF-containing membrane and applied using a film applicator. After application, the glass plate was dried on a hot plate at 60°C for at least 1 hour to evaporate the DMAc, yielding a membrane (hereinafter also referred to as a composite membrane) having a KZnHCF-containing cation exchange layer and a SPES-based cation exchange layer. The obtained composite membrane was immersed in ion-exchange water and peeled from the glass plate.

[0040] Example 6 A composite membrane was obtained in the same manner as in Example 5, except that the blending ratio (mass ratio) of KZnHCF to PES, KZnHCF:PES, was set to 1.5:1.

[0041] Example 7 A composite membrane was obtained in the same manner as in Example 6, except that the cation exchange layer made of SPES was made thicker than in Example 6.

[0042] Example 8 A composite membrane was obtained in the same manner as in Example 5, except that the blending ratio (mass ratio) of KZnHCF and PES, KZnHCF:PES, was set to 2.0:1.

[0043] (Film Thickness Measurement) The film thickness of the obtained film was measured using a film thickness meter (ABS Digimatic Blade Thickness, Mitutoyo Corporation).

[0044] (Measurement of membrane resistance) Figure 7 shows the measurement device and measurement conditions for membrane resistance. First, a platinum electrode with a current-carrying area of ​​0.949 cm 2 NH3 as the measurement solution in an acrylic cell 4 Cl aqueous solution (NH 4 The solution resistance (R 0 After that, the sample film was sandwiched between the two cells, and the resistance (R 1The membrane resistance (R m ) is calculated from the following formula (1), and the obtained membrane resistance is divided by the membrane thickness to obtain the membrane specific resistance K m [Ωcm] was calculated. 1 [Ω cm 2 ] is the resistance measured by sandwiching the sample film between two cells, and R 0 [Ω cm 2 ] is the solution resistance measured without sandwiching the sample film, and R m [Ω cm 2 ] is the membrane resistance. m [Ωcm] is the film resistivity, and d [cm] is the film thickness.

[0045]

[0046]

[0047] (Electrodialysis) As shown in Figure 8, the effective membrane area is 4.0 cm 2 The measurement membrane was sandwiched between two (2.0 cm x 2.0 cm) devices, and the sample was placed in a 0.1 M NH 4 Cl, 0.1 M NaCl and 0.2 M CaCl 2 The mixed salt solution was placed in two cells, and electrodialysis was carried out between Ag / AgCl electrodes at a constant current of 90 mA using a DC stabilized power supply (PMC35-2A, Kikusui Electronics Co., Ltd.) for approximately 120 minutes, and the solution in the cells was sampled at predetermined intervals. After that, the NH 4+ , Na + and Ca 2+ The concentration of these ions was quantified to measure the change in the concentration of these ions over time. From these values, the flux of each ion was calculated using the following formula: In formula (3), J i [mol m -2 ・s -1 ] represents the permeation flux, and V [m 3 ] represents the volume of the concentrated solution, and S [m 2 ] represents the effective membrane area, t [s] represents the time during which the current is passed, and ΔC i / Δt [mol m -3 ・s -1 ] represents the initial concentration gradient. 4+ , Na + or Ca 2+ In formulas (4) and (5), P NH4 Na and P NH4 Ca represents the ion selective permeability coefficient [-]. In formula (6), η [-] represents the current efficiency, and z i [-] represents the valence of the cation, I [A] represents the current, and F [C mol -1 ] represents the Faraday constant. Here, the effective membrane area is the membrane area through which ions actually permeate.

[0048]

[0049]

[0050]

[0051]

[0052] (Measurement Results of Example 1) The thickness of the KCuHCF membrane obtained in Example 1 was 61 μm, and the membrane resistivity of this membrane was 1885 Ωcm and the membrane resistance was 11.5 Ωcm. 2 The results of electrodialysis using this membrane are shown in Figure 9. 4 + , Na + and Ca 2+ The graph shows the time change in ion concentration on the concentrated side and diluted side of the ion. All three types of cations move from the diluted side to the concentrated side due to the applied DC voltage. The permeation flux was calculated from the slope of the time-concentration curve using equation (3), and the ion selectivity coefficient was calculated using equations (4) and (5). As a result, P NH4 Na becomes 1.86, and P NH4 Ca became 1.46. This is Na + 1.86 times more NH 4 + This indicates that Ca selectively permeated the 2+ 1.46 times more NH 4 + This indicates that the current efficiency was 0.82.

[0053] (Measurement Results of Example 2) The thickness of the KZnHCF membrane obtained in Example 2 was 36 μm, and the membrane resistivity of this membrane was 937 Ωcm and the membrane resistance was 3.37 Ωcm. 2 The results of electrodialysis using this membrane are shown in Figure 10. 4 + , Na + and Ca 2+ The graph shows the time change in ion concentration on the concentrated side and diluted side of the ion. All three types of cations move from the diluted side to the concentrated side due to the applied DC voltage. The permeation flux was calculated from the slope of the time-concentration curve using equation (3), and the ion selectivity coefficient was calculated using equations (4) and (5). As a result, P NH4 Na becomes 13.5, and P NH4 Ca was 34.2. This is Na + 13.5 times more NH 4 + This indicates that Ca selectively permeated the 2+ 34.2 times more NH 4 + This indicates that the current efficiency was 0.89.

[0054] (Measurement Results of Example 3) The KZnHCF membrane obtained in Example 3 had a thickness of 45 μm, a membrane resistivity of 416 Ωcm, and a membrane resistance of 1.86 Ωcm. 2 The results of electrodialysis using this membrane are shown in Figure 11. 4 + , Na + and Ca 2+ The graph shows the time change in ion concentration on the concentrated side and diluted side of the ion. All three types of cations move from the diluted side to the concentrated side due to the applied DC voltage. The permeation flux was calculated from the slope of the time-concentration curve using equation (3), and the ion selectivity coefficient was calculated using equations (4) and (5). As a result, P NH4 Na becomes 34.6, and P NH4 Ca The result was 40.4. This is Na + 34.6 times more NH 4+ This indicates that Ca selectively permeated the 2+ 40.4 times more NH 4 + This indicates that the current efficiency was 0.88.

[0055] (Measurement Results of Example 4) The KZnHCF membrane obtained in Example 4 had a thickness of 57 μm, a membrane resistivity of 93 Ωcm, and a membrane resistance of 0.53 Ωcm. 2 The results of electrodialysis using this membrane are shown in Figure 12. 4 + , Na + and Ca 2+ The graph shows the time change in ion concentration on the concentrated side and diluted side of the ion. All three types of cations move from the diluted side to the concentrated side due to the applied DC voltage. The permeation flux was calculated from the slope of the time-concentration curve using equation (3), and the ion selectivity coefficient was calculated using equations (4) and (5). As a result, P NH4 Na becomes 4.2, and P NH4 Ca became 4.2. This is Na + 4.2 times more NH 4 + This indicates that Ca selectively permeated the 2+ 4.2 times more NH 4 + This indicates that the current efficiency was 0.52.

[0056] (Measurement Results of Example 5) The composite membrane obtained in Example 5 had a KZnHCF membrane thickness of 49 μm and a SPES membrane thickness of 24 μm, and the combined membrane specific resistance of the entire membrane was 272 Ωcm and the membrane resistance was 1.99 Ωcm. 2 The results of electrodialysis using this membrane are shown in Figure 13. In Example 5, electrodialysis was carried out by placing the composite membrane so that the SPES membrane faced the cathode. 4 + , Na + and Ca 2+The graph shows the time change in ion concentration on the concentrated side and diluted side of the ion. All three types of cations move from the diluted side to the concentrated side due to the applied DC voltage. The permeation flux was calculated from the slope of the time-concentration curve using equation (3), and the ion selectivity coefficient was calculated using equations (4) and (5). As a result, P NH4 Na becomes 9.0, and P NH4 Ca was 26.3. This is Na + 9.0 times more NH 4 + This indicates that Ca selectively permeated the 2+ 26.3 times more NH 4 + The results show that the current efficiency at this time was 0.94. The composite membrane obtained in Example 5 had a higher current efficiency than the membrane obtained in Example 2. The mechanical strength was also improved.

[0057] (Measurement Results of Example 6) The composite membrane obtained in Example 6 had a KZnHCF membrane thickness of 45 μm and a SPES membrane thickness of 14 μm, and the combined membrane specific resistance of the entire membrane was 550 Ωcm and the membrane resistance was 3.05 Ωcm. 2 In Example 6, electrodialysis was performed by placing the composite membrane so that the SPES membrane faced the cathode. The ion selectivity coefficient was calculated in the same manner as in Example 5. As a result, P NH4 Na becomes 15.0, and P NH4 Ca The current efficiency was 0.95.

[0058] (Measurement Results of Example 7) The composite membrane obtained in Example 7 had a KZnHCF membrane thickness of 45 μm and a SPES membrane thickness of 42.7 μm. The combined membrane specific resistance of the entire membrane was 348 Ωcm, and the membrane resistance was 3.06 Ωcm. 2 In Example 7, electrodialysis was performed by placing the composite membrane so that the SPES membrane faced the cathode. The ion selectivity coefficient was calculated in the same manner as in Example 5. As a result, P NH4 Na becomes 13.3, and P NH4 CaThe current efficiency was 0.94.

[0059] (Measurement Results of Example 8) The composite membrane obtained in Example 8 had a KZnHCF membrane thickness of 58 μm and a SPES membrane thickness of 19 μm, and the combined membrane specific resistance of the entire membrane was 197 Ωcm, and the membrane resistance was 1.52 Ωcm. 2 In Example 8, electrodialysis was performed by placing the composite membrane so that the SPES membrane faced the cathode. The ion selectivity coefficient was calculated in the same manner as in Example 5. As a result, P NH4 Na becomes 12.6, and P NH4 Ca The current efficiency was 10.3.

[0060] [Example 9] In Example 9, the composite membrane obtained in Example 5 was installed so that the SPES membrane faced the anode side, and electrodialysis was carried out. The results are shown in Figure 14. This figure shows the results of electrodialysis using NH 4 + , Na + and Ca 2+ The graph shows the time change in ion concentration on the concentrated side and diluted side of the ion. All three types of cations move from the diluted side to the concentrated side due to the applied DC voltage. The permeation flux was calculated from the slope of the time-concentration curve using equation (3), and the ion selectivity coefficient was calculated using equations (4) and (5). As a result, P NH4 Na becomes 2.4, and P NH4 Ca became 3.3. This is Na + 2.4 times more NH 4 + This indicates that Ca selectively permeated the 2+ 3.3 times more NH 4 + This indicates that the current efficiency was 0.87.

[0061] [Comparative Example] As a comparative example, a standard cation exchange membrane, CSE, manufactured by Astom Co., Ltd., was used and electrodialysis was carried out under the same conditions as in the example. The membrane thickness was 160 μm, and the membrane specific resistance was 113 Ωcm and the membrane resistance was 1.80 Ωcm. 2The results of electrodialysis using this membrane are shown in Figure 15. NH4 Na becomes 1.81, and P NH4 Ca The current efficiency was 0.97. + 1.81 times more NH 4 + This shows that P selectively permeated through this membrane. NH4 Ca Since the value of is less than 1, NH 4 + More than Ca 2+ This indicates that the selective permeation was 1.02 times greater.

[0062] In Examples 5 to 8, a cation exchange layer containing no metal cyano complex was provided on one side of a cation exchange layer containing a metal cyano complex and a binder resin, thereby reducing the amount of Na + and Ca 2+ NH 4 + While maintaining the excellent permselectivity (an ion permselectivity coefficient of more than 10 can be said to be excellent), the current efficiency could be increased.

[0063] The cation exchange membrane of the present invention has excellent selective permeability for ammonium ions and can therefore be used in various applications for concentrating ammonium ions, such as in various water treatments for wastewater, etc. The cation exchange membrane of the present invention can also be suitably used in electrodialysis devices, Donnan dialysis devices, etc.

Claims

1. A cation exchange membrane having a cation exchange layer containing a metal cyano complex and a binder resin.

2. The cation exchange membrane according to claim 1, wherein the mass ratio of the metal cyano complex to the binder resin is from 0.2:1 to 5:

1.

3. Film resistance is 0.2 to 15 Ωcm 2 3. The cation exchange membrane according to claim 1 or 2, 4. The cation exchange membrane according to any one of claims 1 to 3, wherein the binder resin is a resin having no ion exchange capacity and / or a resin having low ion exchange capacity.

5. The cation exchange membrane according to claim 4, wherein the resin having low ion exchange capacity has an ion exchange capacity of 0.001 to 0.2 meq / g.

6. The cation exchange membrane according to any one of claims 1 to 5, which has, on one or both sides of a cation exchange layer containing a metal cyano complex and a binder resin, another cation exchange layer not containing a metal cyano complex.

7. An ion exchange membrane cell comprising an anion exchange membrane and a cation exchange membrane according to any one of claims 1 to 6 arranged opposite each other.

8. An electrodialysis apparatus comprising an anode, a cathode, a cation exchange membrane and an anion exchange membrane, wherein the cation exchange membrane is the cation exchange membrane according to any one of claims 1 to 6.

9. A method for producing a cation exchange membrane, comprising mixing metal cyano complex particles, a binder resin and a solvent, dispersing the metal cyano complex particles in the mixed solution, and then coating or casting the mixed solution to remove the solvent.

10. A method for producing a cation exchange membrane, comprising mixing metal cyano complex particles, a binder resin and a solvent, dispersing the metal cyano complex particles in the mixed solution, applying or casting the mixed solution to a cation exchange layer to remove the solvent, and then applying a mixture of a resin that forms another cation exchange layer not containing a metal cyano complex and a solvent to the cation exchange layer, and removing the solvent, or adhering another cation exchange membrane not containing a metal cyano complex.

Citation Information

Patent Citations

  • Production of ion exchanger

    JP1978123390A

  • Ion exchange paper and preparation of ion exchange body and ion exchange paper

    JP1988001452A

  • Method of treating and recovering cation, and material and treating apparatus used for the same

    JP2011200856A

  • Manufacturing method of aqueous solution containing ammonium ion or / and ammonia, manufacturing method of ammonium salt, and manufacturing apparatus therefor

    JP2019034273A

  • Ammonia chemical species elimination method using carbon dioxide, ammonia chemical species-supplying agent, and ammonia chemical species adsorption and elimination device

    WO2020080302A1