Resin composition, resin composition for metal surface treatment, method for producing metal laminate, and metal laminate

The combination of a solid epoxy resin with polyether polyurethane prepolymers in a water-based resin composition addresses the adhesion issues of current metal surface treatments, providing enhanced adhesion and corrosion resistance for metal bonding applications while minimizing environmental impact.

WO2024203515A1PCT designated stage expired Publication Date: 2024-10-03ADEKA CORP
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010462
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-18
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current water-based resin compositions and metal surface treatment agents lack sufficient adhesion to metal surfaces, necessitating the development of a resin composition with enhanced adhesive properties.

Method used

A resin composition combining a solid epoxy resin at 25°C with polyether polyurethane prepolymers or polyether polyurethanes, specifically using bisphenol-type epoxy resins and polyalkylene glycols, to improve adhesion and corrosion resistance, particularly for short-time pressure bonding applications.

Benefits of technology

The resin composition achieves excellent adhesiveness and corrosion resistance, enabling strong bonding between metal surfaces and reducing environmental impact through the use of a water-based, low-VOC formulation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

Provided is a resin composition containing: a component (A) which is composed of an epoxy resin that is in a solid state at 25°C; and a component (B) which is composed of one or more compounds selected from the group consisting of a polyether polyurethane prepolymer and a polyether polyurethane. Also provided is a method for producing a metal laminate, the method comprising: a step in which the resin composition is applied to the surface of a first metal plate so as to form a coating film; and a step in which a second metal plate is superposed on the coating film of the first metal plate so as to form a metal laminate.
Need to check novelty before this filing date? Find Prior Art

Description

Resin composition, resin composition for metal surface treatment, method for producing metal laminate plate, and metal laminate plate

[0001] The present invention relates to a resin composition having excellent adhesive properties.

[0002] Epoxy resins and urethane resins have excellent adhesion to various substrates and can produce cured products that are excellent in corrosion resistance, heat resistance, chemical resistance, electrical properties, mechanical properties, and the like. Therefore, they are widely used in various fields as adhesives, coating agents, paints, and the like. In recent years, there has been a demand for adhesives, paints, coating agents, and the like containing epoxy resins and urethane resins to be aqueous resin compositions using water as a solvent, from the standpoints of reducing environmental impact and safety. As such aqueous resin compositions, Patent Document 1 describes an environmentally friendly aqueous epoxy resin emulsion that is excellent in storage stability and rust prevention properties, and an aqueous paint containing the same. Patent Document 2 describes an aqueous epoxy resin dispersion with low volatile organic compounds (VOCs), particularly for coating metals and concrete.

[0003] Furthermore, various metal surface treatment agents using aqueous epoxy resins and the like that have metal adhesion and corrosion prevention properties have also been developed. For example, Patent Document 3 describes an aqueous coating composition that can improve the water-resistant adhesion to steel sheets that have been subjected to surface treatments such as plating, and form a coating film that exhibits excellent corrosion resistance and corrosion prevention. Patent Document 4 describes a surface treatment agent for metal materials that can produce surface-treated metal materials with coating films that have excellent corrosion resistance, adhesion, etc., even when primer painting is omitted.

[0004] JP 2014-009270 A JP 2015-214698 A JP 2015-124234 A WO 2015 / 056355

[0005] However, these aqueous resin compositions and metal surface treatment agents do not have sufficient adhesiveness to metal surfaces, etc., and there has been a demand in the market for resin compositions with excellent adhesiveness.

[0006] In view of the above circumstances, an object of the present invention is to provide a resin composition having excellent adhesive properties.

[0007] The present inventors conducted extensive research and found that a resin composition containing specific components can solve the above problems. That is, the present invention provides a resin composition containing component (A) consisting of an epoxy resin that is solid at 25°C and component (B) consisting of one or more members selected from the group consisting of polyether polyurethane prepolymers and polyether polyurethanes.

[0008] According to the present invention, a resin composition having excellent adhesive properties can be provided.

[0009] 1. Resin Composition The resin composition of the present invention is a resin composition containing component (A) consisting of an epoxy resin that is solid at 25°C, and component (B) consisting of one or more components selected from the group consisting of polyether polyurethane prepolymers and polyether polyurethanes. The resin composition of the present invention will be described in detail below. 1-1. Component (A) Component (A) used in the present invention consists of an epoxy resin that is solid at 25°C. In the present invention, there are no particular limitations on the epoxy resin that can be used as long as it is solid at 25°C. Examples of such epoxy resins include bisphenol-type epoxy resins such as bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, bisphenol S-type epoxy resins, and bisphenol AD-type epoxy resins, which are solid at 25°C, resorcinol-type epoxy resins, hydroquinone-type epoxy resins, catechol-type epoxy resins, dihydroxynaphthalene-type epoxy resins, biphenyl-type epoxy resins, tetramethylbiphenyl-type epoxy resins, oxazolidone ring-type epoxy resins, phenol novolac-type epoxy resins, cresol novolac-type epoxy resins, triphenylmethane-type epoxy resins, tetraphenylethane-type epoxy resins, dicyclopentadiene-phenol addition reaction-type epoxy resins, phenol aralkyl-type epoxy resins, naphthol novolac-type epoxy resins, naphthol aralkyl-type epoxy resins, naphthol-phenol co-condensed novolac-type epoxy resins, naphthol-cresol co-condensed novolac-type epoxy resins, aromatic hydrocarbon formaldehyde resin-modified phenolic resin-type epoxy resins, and biphenyl-modified novolac-type epoxy resins. One or more of these may be used. Among these, from the viewpoint of improving the adhesiveness of the resulting resin composition, particularly the adhesiveness after pressure bonding in a short time, it is preferable to use a bisphenol type epoxy resin that is solid at 25°C, it is more preferable to use one or more resins selected from the group consisting of bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, and bisphenol AD ​​type epoxy resins that are solid at 25°C, and it is even more preferable to use a bisphenol A type epoxy resin that is solid at 25°C.In the present invention, being solid at 25°C means that the melting point is higher than 25°C and that the epoxy resin is solid at 25°C. The melting point of the epoxy resin is not particularly limited as long as it is higher than 25°C. From the viewpoint of the adhesiveness of the resulting resin composition, the melting point of the epoxy resin is preferably 40°C to 180°C, and more preferably 70°C to 150°C. Furthermore, component (A) consisting of an epoxy resin that is solid at 25°C does not include the phosphoric acid-modified epoxy resin described below and is clearly distinguished from it.

[0010] The epoxy equivalent of the epoxy resin in a solid state at 25°C is not particularly limited and can be adjusted according to the purpose. From the viewpoint of improving the adhesiveness of the resulting resin composition, particularly adhesiveness by short-term pressure bonding, the epoxy equivalent of the epoxy resin in a solid state at 25°C is preferably 500 g / eq. to 30,000 g / eq., more preferably 1,000 g / eq. to 10,000 g / eq., even more preferably 1,500 g / eq. to 6,000 g / eq., even more preferably 2,000 g / eq. to 5,000 g / eq., and particularly preferably 2,500 g / eq. to 3,500 g / eq. In the present invention, the epoxy equivalent of the epoxy resin is measured in accordance with JIS K 7236 (2009).

[0011] 1-2. Component (B) Component (B) used in the present invention comprises one or more compounds selected from the group consisting of polyether polyurethane prepolymers and polyether polyurethanes. In the present invention, the term "polyether polyurethane prepolymer" refers to a compound obtained by reacting raw materials containing at least one polyether polyol compound and at least one polyisocyanate compound in such a manner that unreacted isocyanate groups remain in the compound. Furthermore, in the present invention, the term "polyether polyurethane" refers to a compound obtained by reacting raw materials containing at least one polyether polyol compound and at least one polyisocyanate compound in such a manner that unreacted isocyanate groups remain in the compound, or by capping the polyether polyurethane prepolymer obtained by the above-described method with a capping agent or by chain-extending the prepolymer with a chain extender.

[0012] In the present invention, examples of polyether polyol compounds that can be used in the production of polyether polyurethane prepolymers include polyalkylene glycols such as polyethylene glycol, polypropylene glycol, polytetramethylene ether glycol, polyethylene glycol-polypropylene glycol random copolymers, and polyethylene glycol-polypropylene glycol block copolymers, as well as polyoxyethylene adducts, polyoxypropylene adducts, and polyoxybutylene adducts of diol compounds such as ethylene glycol, propanediol, and butanediol. Among these, from the viewpoint of the adhesiveness and corrosion resistance of the resulting resin composition, it is preferable to use one or more polyalkylene glycols, more preferably one or more selected from the group consisting of polyethylene glycol, polypropylene glycol, and polytetramethylene ether glycol, even more preferably one or more selected from the group consisting of polypropylene glycol and polytetramethylene ether glycol, and particularly preferably polytetramethylene ether glycol. The molecular weight of the polyether polyol compound used is not particularly limited. From the viewpoint of the adhesiveness and corrosion resistance of the resulting resin composition, it is preferable to use a polyether polyol compound having a number average molecular weight of 200 to 10,000, more preferably a polyether polyol compound having a number average molecular weight of 400 to 5,000, even more preferably a polyether polyol compound having a number average molecular weight of 600 to 2,000, and particularly preferably a polyether polyol compound having a number average molecular weight of 800 to 1,500. In the present invention, the number average molecular weight of the polyether polyol compound is measured by gel permeation chromatography (GPC) and is the number average molecular weight calculated in terms of polystyrene.

[0013] In the present invention, the polyisocyanate compound that can be used in the production of the polyether polyurethane prepolymer is not particularly limited as long as it has two or more isocyanate groups in the molecule. Examples of such polyisocyanate compounds include aromatic diisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, hydrogenated diphenylmethane diisocyanate, p-phenylene diisocyanate, xylylene diisocyanate, 1,5-naphthylene diisocyanate, 3,3'-dimethyldiphenyl-4,4'-diisocyanate, dianisidine diisocyanate, and tetramethylxylylene diisocyanate; alicyclic diisocyanates such as isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, trans-1,4-cyclohexyl diisocyanate, and norbornene diisocyanate; and 1,4-tetramethylxylylene diisocyanate. Examples of the diisocyanate include aliphatic diisocyanates such as lamethylene diisocyanate, 1,6-hexamethylene diisocyanate, 1,8-octamethylene diisocyanate, 2-methyl-1,5-pentamethylene diisocyanate, 2,2-dimethyl-1,5-pentamethylene diisocyanate, 1,11-undecamethylene diisocyanate, 2,2,4-trimethyl-1,6-hexamethylene diisocyanate, 2,4,4-trimethyl-1,6-hexamethylene diisocyanate, 2,4-dimethyl-1,8-octamethylene diisocyanate, 5-methyl-1,9-nonamethylene diisocyanate, lysine diisocyanate, and lysine methyl ester diisocyanate. In addition, in producing the polyether polyurethane prepolymer, as the polyisocyanate compound, an isocyanurate trimer, a biuret trimer, or a trimethylolpropane adduct of the above-mentioned diisocyanate compound, or a polyisocyanate compound having three or more isocyanate groups in the molecule, such as triphenylmethane triisocyanate, 1-methylbenzene-2,4,6-triisocyanate, or dimethyltriphenylmethane tetraisocyanate, can also be used.In the present invention, from the viewpoint of the adhesiveness and corrosion resistance of the resulting resin composition, it is preferable to use one or more selected from the group consisting of aromatic diisocyanates, alicyclic diisocyanates, and aliphatic diisocyanates, and it is more preferable to use one or more selected from the group consisting of tolylene diisocyanate, diphenylmethane diisocyanate, hydrogenated diphenylmethane diisocyanate, p-phenylene diisocyanate, xylylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, and 1,6-hexamethylene diisocyanate, and it is even more preferable to use one or more selected from the group consisting of hydrogenated diphenylmethane diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, and 1,6-hexamethylene diisocyanate.

[0014] The polyether polyurethane prepolymer that can be used in the present invention is not particularly limited, as long as it is obtained by reacting raw materials containing at least one polyether polyol compound and at least one polyisocyanate compound so that unreacted isocyanate groups remain. For example, a polyether polyurethane prepolymer obtained by reacting raw materials containing the above-mentioned polyether polyol compound and polyisocyanate compound in amounts such that the ratio of the number of hydroxyl groups in the polyether polyol compound to the number of isocyanate groups in the polyisocyanate compound is 0.20 to 0.99:1 can be used.

[0015] Furthermore, the polyether polyurethane prepolymer used in the present invention may be a compound obtained by reacting at least one polyether polyol compound, at least one polyisocyanate compound, and one or more raw materials having a reactive group such as a hydroxyl group or an amino group that can react with the polyisocyanate compound, such as an anionic group-introducing agent, a melamine compound, or a low-molecular-weight polyol, in such a manner that unreacted isocyanate groups remain in the compound.

[0016] The anionic group introducing agent that can be used in the production of the polyether polyurethane prepolymer is not particularly limited, as long as it contains, in the molecule, an anionic group such as a carboxyl group or a sulfonic acid group, and a reactive group such as a hydroxyl group or an amino group that can react with a polyisocyanate compound. Examples of such anionic group introducing agents include compounds containing a carboxyl group and a hydroxyl group, such as dimethylolpropionic acid, dimethylolbutanoic acid, dimethylolbutyric acid, and dimethylolvaleric acid; and compounds containing a sulfonic acid group and a hydroxyl group, such as 1,4-butanediol-2-sulfonic acid. One or more of these can be used. Among these, in the present invention, from the viewpoint of the adhesiveness and corrosion resistance of the resulting resin composition, it is preferable to use, as the anionic group-introducing agent, a compound having a carboxyl group and a hydroxyl group in the molecule, it is more preferable to use a compound having a carboxyl group and a hydroxyl group in the molecule and having a molecular weight of 100 to 5,000, it is even more preferable to use dimethylolpropionic acid or dimethylolbutanoic acid, and it is particularly preferable to use dimethylolpropionic acid.

[0017] In the present invention, when an anionic group-introducing agent is used in producing a polyether polyurethane prepolymer, the amount of the anionic group-introducing agent used is not particularly limited and can be adjusted appropriately depending on the purpose. For example, the anionic group-introducing agent can be used in an amount such that, when the number of isocyanate groups in the polyisocyanate compound used is 1, the number of reactive groups in the anionic group-introducing agent that can react with the polyisocyanate compound, such as hydroxyl groups and amino groups, is 0.01 to 0.80, preferably 0.05 to 0.60, and more preferably 0.10 to 0.50.

[0018] Furthermore, when an anionic group-introducing agent is used in the production of a polyether polyurethane prepolymer, the amount of the anionic group-introducing agent relative to the polyether polyol compound is not particularly limited and can be adjusted appropriately depending on the purpose. For example, when the number of reactive groups, such as hydroxyl groups and amino groups, that can react with a polyisocyanate compound in the polyether polyol compound used is taken as 1, the anionic group-introducing agent can be used in an amount such that the number of reactive groups, such as hydroxyl groups and amino groups, that can react with a polyisocyanate compound in the anionic group-introducing agent is 0.05 to 20, preferably 0.1 to 10, and more preferably 0.2 to 5.

[0019] Examples of melamine-based compounds that can be used in producing the polyether polyurethane prepolymer include melamine, monomethylolmelamine, dimethylolmelamine, trimethylolmelamine, tetramethylolmelamine, pentamethylolmelamine, hexamethylolmelamine, methylated methylolmelamine, butylated methylolmelamine, and melamine resins. One or more of these compounds can be used. Among these, in the present invention, from the viewpoint of the adhesiveness and corrosion resistance of the resulting resin composition, it is preferable to use one or more compounds selected from the group consisting of melamine, monomethylolmelamine, and dimethylolmelamine, and it is more preferable to use melamine.

[0020] In the present invention, when a melamine-based compound is used in the production of a polyether polyurethane prepolymer, the amount of the melamine-based compound to be used is not particularly limited and can be appropriately adjusted depending on the purpose. For example, the melamine-based compound can be used in an amount such that, when the number of isocyanate groups in the polyisocyanate compound used is 1, the number of amino groups in the melamine-based compound is 0.01 to 0.50, preferably 0.05 to 0.40, and more preferably 0.10 to 0.30.

[0021] Furthermore, when a melamine compound is used to produce a polyether polyurethane prepolymer, the amount of the melamine compound relative to the polyether polyol compound is not particularly limited and can be adjusted appropriately depending on the purpose. For example, when the number of reactive groups, such as hydroxyl groups and amino groups, that can react with a polyisocyanate compound in the polyether polyol compound used is taken as 1, the melamine compound can be used in an amount such that the number of amino groups is 0.05 to 20, preferably 0.1 to 10, and more preferably 0.2 to 5.

[0022] Examples of low molecular weight polyols that can be used in the production of polyether polyurethane prepolymers include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 2-methyl-1,3-propanediol, 2-butyl-2-ethyl-1,3-propanediol, 1,4-butanediol, neopentyl glycol, 3-methyl-2,4-pentanediol, 2,4-pentanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 2-methyl-2,4-pentanediol, and 2,4-diethyl-1,5-pentanediol. aliphatic diols such as cyclohexanedimethanol, cyclohexanediol, and the like; aliphatic diols such as cyclohexanedimethanol, cyclohexanediol, and the like; and trihydric or higher alcohols such as trimethylolethane, trimethylolpropane, hexitols, pentitols, glycerin, pentaerythritol, and tetramethylolpropane. These may be used alone or in combination.

[0023] In the present invention, when a low-molecular-weight polyol is used in producing a polyether polyurethane prepolymer, the amount of the low-molecular-weight polyol used is not particularly limited and can be appropriately adjusted depending on the purpose. For example, when the number of isocyanate groups in the polyisocyanate compound used is taken as 1, the low-molecular-weight polyol can be used in an amount such that the number of reactive groups, such as hydroxyl groups, that can react with the polyisocyanate compound in the low-molecular-weight polyol is 0.01 to 0.50, preferably 0.05 to 0.40, and more preferably 0.10 to 0.30.

[0024] In the present invention, from the viewpoint of the adhesiveness and corrosion resistance of the resulting resin composition, it is preferable to use, as the polyether polyurethane prepolymer, a polyether polyurethane prepolymer obtained using raw materials containing at least one polyether polyol compound, at least one polyisocyanate compound, and one or more compounds selected from the group consisting of an anionic group-introducing agent and a melamine-based compound; it is more preferable to use a polyether polyurethane prepolymer obtained using raw materials containing at least one polyether polyol compound, at least one polyisocyanate compound, at least one anionic group-introducing agent, and at least one melamine-based compound; and it is even more preferable to use a polyether polyurethane prepolymer obtained by reacting raw materials consisting of at least one polyether polyol compound, at least one polyisocyanate compound, at least one anionic group-introducing agent, and at least one melamine-based compound.

[0025] In the present invention, when producing a polyether polyurethane prepolymer using raw materials containing at least one polyether polyol compound, at least one polyisocyanate compound, at least one anionic group-introducing agent, and at least one melamine-based compound, the amounts of the polyether polyol compound, polyisocyanate compound, anionic group-introducing agent, and melamine-based compound used are not particularly limited and can be adjusted appropriately depending on the purpose. From the viewpoint of the adhesiveness and corrosion resistance of the resulting resin composition, for example, when the number of isocyanate groups in the polyisocyanate compound is taken as 1, the sum of the number of reactive groups such as hydroxyl groups in the polyether polyol compound, the number of reactive groups such as hydroxyl groups in the anionic group-introducing agent, and the number of amino groups in the melamine-based compound is preferably used in an amount such that the sum is 0.20 to 0.99, more preferably 0.30 to 0.95, and even more preferably 0.40 to 0.90.

[0026] In addition, when a polyether polyurethane prepolymer is produced using raw materials containing at least one polyether polyol compound, at least one polyisocyanate compound, at least one anionic group introducing agent, and at least one melamine-based compound, the amounts of the polyether polyol compound, the polyisocyanate compound, the anionic group introducing agent, and the melamine-based compound to be used are determined based on the amount of isocyanates in the polyisocyanate compound from the viewpoint of adhesiveness and corrosion resistance of the resulting resin composition. The anionic group-introducing agent is preferably used in an amount such that the ratio of the number of anate groups, the number of reactive groups such as hydroxyl groups in the polyether polyol compound, the number of reactive groups such as hydroxyl groups in the anionic group-introducing agent, and the number of amino groups in the melamine compound is 1:0.01-0.9:0.01-0.9:0.01-0.5, more preferably 1:0.05-0.6:0.05-0.6:0.05-0.4, and even more preferably 1:0.1-0.5:0.1-0.5:0.05-0.3.

[0027] The acid value of the polyether polyurethane prepolymer that can be used in the present invention is not particularly limited and can be adjusted appropriately depending on the purpose. From the viewpoint of the adhesiveness and corrosion resistance of the resulting resin composition, the acid value of the polyether polyurethane prepolymer is preferably 0 to 70 mgKOH / g, more preferably 10 to 60 mgKOH / g, even more preferably 15 to 50 mgKOH / g, and particularly preferably 20 to 40 mgKOH / g. In the present invention, the acid value of the polyether polyurethane prepolymer is a value measured by the neutralization titration method of JIS K 0070 (1992).

[0028] The polyether polyurethane prepolymer used in the present invention is not particularly limited, and can be produced by charging the above-mentioned raw materials, either all at once or in multiple batches, into a reaction vessel in the presence of a solvent, a catalyst, etc. as necessary, and mixing and reacting them for 10 minutes to 24 hours, for example, at room temperature to 180°C and at 0.01 Pa to 100 MPa. At this time, by carrying out the reaction using a polyisocyanate compound contained in the raw materials so that the number of isocyanate groups in the compound is greater than the number of reactive groups, such as hydroxyl groups and amino groups, that can react with the isocyanate groups contained in raw materials such as a polyether polyol compound, a polyether polyurethane prepolymer having unreacted isocyanate groups can be produced.

[0029] The catalyst that can be used in producing the polyether polyurethane prepolymer is not particularly limited, and known catalysts can be used. Examples of such catalysts include N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethylpropylenediamine, N,N,N',N",N"-pentamethyldiethylenetriamine, N,N,N',N",N"-pentamethyl(3-aminopropyl)ethylenediamine, N,N,N',N",N"-pentamethyldipropylenetriamine, N,N,N',N'-tetramethylguanidine, 1,3,5 -tris(N,N-dimethylaminopropyl)hexahydro-S-triazine, 1,8-diazabicyclo[5.4.0]undecene-7, triethylenediamine, N,N,N',N'-tetramethylhexamethylenediamine, N-methyl-N'-(2-dimethylaminoethyl)piperazine, N,N'-dimethylpiperazine, N,N-dimethylcyclohexylamine, N-methylmorpholine, N-ethylmorpholine, bis(2-dimethylaminoethyl) Tertiary amines such as tertiary amines (e.g., methylaminoethyl) ether, N,N-dimethyllaurylamine, 1-methylimidazole, 1,2-dimethylimidazole, 1-isobutyl-2-methylimidazole, and 1-dimethylaminopropylimidazole; quaternary ammonium salts such as tetraalkylammonium halides (e.g., tetramethylammonium chloride), tetraalkylammonium hydroxides (e.g., tetramethylammonium hydroxide salt), and tetraalkylammonium organic acid salts (e.g., tetramethylammonium 2-ethylhexanoate); and organometallic catalysts such as stannous diacetate, stannous dioctoate, stannous dioleate, stannous dilaurate, dibutyltin oxide, dibutyltin diacetate, dibutyltin dilaurate, dibutyltin dichloride, dioctyltin dilaurate, lead octoate, lead naphthenate, nickel naphthenate, and cobalt naphthenate. These catalysts may be used alone or in combination. The amount of catalyst used is not particularly limited and can be adjusted appropriately depending on the purpose. The catalyst can be used in an amount of, for example, 0.0001 to 1% by mass based on the total mass of the raw materials used.

[0030] Known solvents can be used when producing the polyether polyurethane prepolymer. Examples of such solvents include acetone, methyl ethyl ketone, dioxane, tetrahydrofuran, N-methyl-2-pyrrolidone, ethylene glycol monomethyl ether, propylene glycol monomethyl ether, ethylene glycol monomethyl ether acetate, and propylene glycol monomethyl ether acetate. One or more of these can be used. The amount of solvent used is not particularly limited and can be adjusted appropriately depending on the purpose. The solvent can be used in an amount of, for example, 0.1 to 80% by mass relative to the total mass of the raw materials used.

[0031] In the present invention, the reaction time when the polyether polyol compound, the polyisocyanate compound, and other raw materials are reacted to produce the polyether polyurethane prepolymer is not particularly limited. From the viewpoint of the adhesiveness and corrosion resistance of the resulting resin composition, the reaction time is preferably 30 minutes to 15 hours, more preferably 1 hour to 10 hours, and even more preferably 3 hours to 7 hours.

[0032] The polyether polyurethane prepolymer obtained by the above-mentioned method is obtained by reacting a polyether polyol compound, a polyisocyanate compound, and, if necessary, an anionic group-introducing agent and a melamine-based compound. In the present invention, a wide variety of compounds can be used as the polyether polyol compound, the polyisocyanate compound, the anionic group-introducing agent, and the melamine-based compound. Therefore, the structure of the polyether polyurethane prepolymer varies significantly depending on the structure of the raw materials used to produce the polyether polyurethane prepolymer. Therefore, it is currently impossible to uniformly express the structure of a polyether polyurethane prepolymer with a certain general formula, and this is common technical knowledge among those skilled in the art. Furthermore, without a specified structure, the properties of the substance, which are determined accordingly, cannot be easily determined, and therefore cannot be expressed in terms of properties. On the other hand, the present invention relates to the discovery that a polyether polyurethane prepolymer obtained by reacting raw materials containing at least one polyether polyol compound and at least one polyisocyanate compound can produce a resin composition having excellent adhesive properties, particularly adhesive properties that allow bonding with short periods of pressure bonding, and corrosion resistance, when used in combination with component (A) consisting of an epoxy resin that is solid at 25° C. Therefore, in the present invention, the polyether polyurethane prepolymer must be defined as "a polyether polyurethane prepolymer obtained by reacting raw materials containing at least one polyether polyol compound and at least one polyisocyanate compound."

[0033] Examples of polyether polyurethanes that can be used in the present invention include polyether polyurethanes obtained by blocking the polyether polyurethane prepolymer obtained by the above-mentioned method with a blocking agent or by chain extending the prepolymer with a chain extender, and polyether polyurethanes obtained by reacting raw materials containing at least one polyether polyol compound and at least one polyisocyanate compound in such a way that no unreacted isocyanate groups remain in the compound.

[0034] In the present invention, the blocking agent used to block the polyether polyurethane prepolymer is not particularly limited, and known blocking agents can be used. Examples of such blocking agents include alcohols such as methanol and ethanol; dialkylamines such as diethylamine, dimethylamine, dipropylamine, dibutylamine, dipentylamine, dihexylamine, didodecylamine, and distearylamine; diarylamines such as diphenylamine; and secondary amino group-containing heterocyclic compounds such as morpholine, piperidine, pyrrole, pyrrolidine, pyrazole, and imidazole. One or more of these can be used. In this case, the amount of the blocking agent used is not particularly limited and can be adjusted appropriately depending on the purpose. For example, the amount can be such that the number of reactive groups in the blocking agent that can react with isocyanate groups relative to the number of isocyanate groups in the polyether polyurethane prepolymer is an equivalent ratio of 0.01 to 2.0.

[0035] In the present invention, the chain extender used for extending the chain of the polyether polyurethane prepolymer is not particularly limited, and known chain extenders can be used. Examples of such chain extenders include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 2-methyl-1,3-propanediol, diethylene glycol, triethylene glycol, 2-butyl-2-ethyl-1,3-propanediol, 1,4-butanediol, neopentyl glycol, 3-methyl-2,4-pentanediol, 2,4-pentanediol, 1,5-pentanediol, and 3-methyl-1,5-pentanediol. aliphatic diols such as pentanediol, 2-methyl-2,4-pentanediol, 2,4-diethyl-1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 3,5-heptanediol, 1,8-octanediol, 2-methyl-1,8-octanediol, and 1,9-nonanediol; alicyclic diols such as cyclohexanedimethanol and cyclohexanediol; ethylenediamine, propylenediamine, hexamethylenediamine, low molecular weight diamines such as diethylenetriamine, tolylenediamine, piperazine, and 2-methylpiperazine; polyalkylenepolyamines such as diethylenetriamine, triethylenetetramine, and tetraethylenepentamine; alkanolamines such as monoethanolamine, diethanolamine, triethanolamine, monoisopropanolamine, diisopropanolamine, triisopropanolamine, and 2-(2-aminoethylamino)ethanol; polyether diamines such as polyoxypropylenediamine and polyoxyethylenediamine; alicyclic diamines such as menthenediamine, isophoronediamine, norbornenediamine, aminoethylaminoethanol, bis(4-amino-3-methyldicyclohexyl)methane, diaminodicyclohexylmethane, bis(aminomethyl)cyclohexane, and 3,9-bis(3-aminopropyl)-2,4,8,10-tetraoxaspiro(5,5)undecane;Examples of suitable aromatic diamines include polyamines such as m-xylenediamine, α-(m / p-aminophenyl)ethylamine, m-phenylenediamine, diaminodiphenylmethane, diaminodiphenylsulfone, diaminodimethyldiphenylmethane, diaminodiethyldiphenylmethane, dimethylthiotoluenediamine, diethyltoluenediamine, and α,α'-bis(4-aminophenyl)-p-diisopropylbenzene; hydrazines such as succinic acid dihydrazide, adipic acid dihydrazide, sebacic acid dihydrazide, phthalic acid dihydrazide, hydrazine hydrate, 1,6-hexamethylenebis(N,N-dimethylsemicarbazide), and 1,1,1',1'-tetramethyl-4,4'-(methylene-di-para-phenylene)disemicarbazide; and water. These may be used alone or in combination. Among these, from the viewpoint of the various properties of the resulting polyether polyurethane, it is preferable to use one or more selected from the group consisting of low-molecular-weight diamines, polyether diamines, and water, and it is more preferable to use one or more selected from the group consisting of ethylene diamine, propylene diamine, and water. In this case, the amount of chain extender used is not particularly limited and can be adjusted appropriately depending on the purpose. For example, the equivalent ratio of the number of reactive groups in the chain extender that can react with isocyanate groups to the number of isocyanate groups in the polyether polyurethane prepolymer can be 0.01 or more. From the viewpoint of the various properties of the resulting polyether polyurethane, it is preferable to set the equivalent ratio to 0.5 or more, and more preferably 1 or more. In the present invention, when water is used as the chain extender, the water also functions as a solvent for the resulting resin composition, so there is no particular upper limit to the amount of the water-containing chain extender used. The water-containing chain extender can be used in an amount of, for example, 10% by mass to 1000% by mass relative to the mass of the polyether polyurethane prepolymer.

[0036] In the present invention, the polyether polyol compound and polyisocyanate compound that can be used to produce a polyether polyurethane by reacting raw materials containing at least one polyether polyol compound and at least one polyisocyanate compound so that no unreacted isocyanate groups remain in the compound can be any known polyether polyol compound and polyisocyanate compound, without any particular limitations. Examples of such polyether polyol compounds and polyisocyanate compounds include the polyether polyol compounds and polyisocyanate compounds that can be used to produce the above-mentioned polyether polyurethane prepolymer. Furthermore, when reacting raw materials containing at least one polyether polyol compound and at least one polyisocyanate compound so that no unreacted isocyanate groups remain in the compound, the ratio of the amounts of the polyether polyol compound and polyisocyanate compound used is not particularly limited and can be adjusted appropriately depending on the purpose. For example, the polyether polyol compound and the polyisocyanate compound can be used in amounts such that the ratio of the number of hydroxyl groups in the polyether polyol compound to the number of isocyanate groups in the polyisocyanate compound is 1:0.5 to 0.99.

[0037] Among these, from the viewpoint of the adhesiveness and corrosion resistance of the resulting resin composition, the polyether polyurethane is preferably a polyether polyurethane obtained by reacting a raw material containing at least one polyether polyol compound and at least one polyisocyanate compound, and then blocking the resulting polyether polyurethane prepolymer with a blocking agent or extending the chains of the resulting polyether polyurethane prepolymer with a chain extender. More preferably, the polyether polyurethane is obtained by using a raw material containing at least one polyether polyol compound, at least one polyisocyanate compound, and one or more compounds selected from the group consisting of an anionic group-introducing agent and a melamine-based compound, and then blocking the resulting polyether polyurethane prepolymer with a blocking agent or extending the chains of the resulting polyether polyurethane prepolymer with a chain extender. The polyether polyurethane is preferably a polyether polyurethane obtained by capping with a capping agent or chain-extending with a chain extender a polyether polyurethane prepolymer obtained using raw materials containing at least one polyether polyol compound, at least one polyisocyanate compound, at least one anionic group-introducing agent, and at least one melamine-based compound, and even more preferably a polyether polyurethane obtained by capping with a capping agent or chain-extending with a chain extender a polyether polyurethane prepolymer obtained by reacting raw materials consisting of at least one polyether polyol compound, at least one polyisocyanate compound, at least one anionic group-introducing agent, and at least one melamine-based compound.

[0038] The acid value of the polyether polyurethane that can be used in the present invention is not particularly limited and can be adjusted appropriately depending on the purpose. From the viewpoint of the adhesiveness and corrosion resistance of the resulting resin composition, the acid value of the polyether polyurethane is preferably 0 to 70 mgKOH / g, more preferably 10 to 60 mgKOH / g, even more preferably 15 to 50 mgKOH / g, and particularly preferably 20 to 40 mgKOH / g. In the present invention, the acid value of the polyether polyurethane is a value measured by the neutralization titration method of JIS K 0070 (1992).

[0039] The polyether polyurethane obtained by the above-mentioned method is obtained by reacting a polyether polyol compound, a polyisocyanate compound, and, if necessary, an anionic group-introducing agent, a melamine-based compound, and a blocking agent or chain extender. In the present invention, a wide variety of compounds can be used as the polyether polyol compound, polyisocyanate compound, anionic group-introducing agent, melamine-based compound, blocking agent, and chain extender. Therefore, since the structure of the polyether polyurethane varies significantly depending on the structure of the raw materials used in the production of the polyether polyurethane, it is currently impossible to uniformly represent the structure of a polyether polyurethane by a certain general formula, and this is common technical knowledge among those skilled in the art. Furthermore, without a specified structure, the properties of the substance, which are determined accordingly, cannot be easily determined, and therefore cannot be expressed in terms of properties. On the other hand, the present invention relates to the discovery that a polyether polyurethane obtained by reacting raw materials containing at least one polyether polyol compound and at least one polyisocyanate compound can produce a resin composition having excellent adhesive properties, particularly adhesive properties that allow bonding with short periods of pressure bonding, and corrosion resistance, when used in combination with component (A) consisting of an epoxy resin that is solid at 25° C. Therefore, in the present invention, polyether polyurethane must be defined as "a polyether polyurethane obtained by reacting raw materials containing at least one polyether polyol compound and at least one polyisocyanate compound."

[0040] The present invention relates to the discovery that when component (B) consisting of one or more selected from the group consisting of the aforementioned polyether polyurethane prepolymer and polyether polyurethane is used in combination with component (A) consisting of an epoxy resin that is solid at 25°C, a resin composition having excellent adhesive properties, particularly adhesive properties that allow bonding with short periods of pressure bonding and corrosion resistance, can be obtained. From the viewpoint of improving adhesive properties and corrosion resistance by using component (A) in combination, particularly adhesive properties that allow bonding with short periods of pressure bonding and corrosion resistance, the content of polyether structures in the polyether polyurethane prepolymer or polyether polyurethane is preferably 10 to 70 mass%, more preferably 15 to 60 mass%, and even more preferably 20 to 50 mass%, relative to the total mass of the polyether polyurethane prepolymer or polyether polyurethane. In the present invention, the content of polyether structures in the polyether polyurethane prepolymer or polyether polyurethane is calculated based on the mass content of polyether structures in the raw materials used.

[0041] The component (B) used in the present invention may consist solely of the above-mentioned polyether polyurethane prepolymer, or may consist solely of polyether polyurethane, or may consist solely of polyether polyurethane prepolymer and polyether polyurethane. From the viewpoint of the properties of the resulting resin composition, it is preferable that the component (B) contains polyether polyurethane.

[0042] The content of component (A) in the resin composition of the present invention is not particularly limited and can be adjusted appropriately depending on the purpose. From the viewpoint of improving the adhesiveness of the resulting resin composition, particularly the adhesiveness by short-term pressure bonding, the content of component (A) in the resin composition is preferably 3 to 60 mass %, more preferably 5 to 50 mass %, even more preferably 8 to 45 mass %, and even more preferably 20 to 40 mass %, based on the total amount of the resin composition.

[0043] The content of component (B) in the resin composition of the present invention is not particularly limited and can be adjusted appropriately depending on the purpose. From the viewpoint of improving the adhesiveness of the resulting resin composition, particularly the adhesiveness by short-term pressure bonding, the content of component (B) in the resin composition is preferably 1 to 50 mass %, more preferably 2 to 40 mass %, even more preferably 3 to 30 mass %, and particularly preferably 4 to 10 mass %, based on the total amount of the resin composition.

[0044] The content ratio of component (A) to component (B) in the resin composition of the present invention is not particularly limited and can be adjusted depending on the purpose. From the viewpoint of improving the adhesiveness of the resulting resin composition, particularly the adhesiveness by short-term pressure bonding, the content ratio of component (A) to component (B) in the resin composition is preferably 5:95 to 98:2 by mass, more preferably 20:80 to 95:5, even more preferably 50:50 to 92:8, and particularly preferably 70:30 to 90:10.

[0045] 1-3. Water The resin composition of the present invention may further contain water. The water content in the resin composition of the present invention is not particularly limited and can be adjusted as appropriate. From the viewpoints of the adhesion and corrosion resistance of the resin composition to metals, reduction of environmental impact, and ease of handling of the resin composition, the resin composition preferably contains 10 to 90% by mass of water, more preferably 20 to 80% by mass, even more preferably 30 to 70% by mass, and particularly preferably 40 to 60% by mass, of the total amount of water. In this case, tap water, ion-exchanged water, distilled water, natural water, pure water, etc. can be used as the water, as appropriate, depending on the purpose.

[0046] When the resin composition of the present invention contains water, the ratio of the contents of component (A), component (B), and water is not particularly limited and can be adjusted according to the purpose. From the viewpoints of the adhesion and corrosion resistance of the resin composition to metal, reduction in environmental load, and ease of handling of the resin composition, the ratio of the contents of component (A), component (B), and water in the resin composition is preferably 3 to 80:1 to 60:10 to 90, more preferably 5 to 60:2 to 50:20 to 80, even more preferably 8 to 50:3 to 40:30 to 70, and particularly preferably 20 to 40:4 to 10:40 to 60. By containing the specific components (A), (B), and water in such a content ratio, the resin composition of the present invention can obtain a water-dispersed emulsion having excellent dispersion stability as a resin composition, thereby reducing the environmental load and making it easy to handle.

[0047] When the resin composition of the present invention contains water, it is preferable to use, as component (A), a bisphenol-type epoxy resin that is solid at 25° C. among the above-mentioned epoxy resins that are solid at 25° C., from the viewpoint of the dispersion stability and various properties of the resulting resin composition, more preferably one or more selected from the group consisting of bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, bisphenol S-type epoxy resins, and bisphenol AD-type epoxy resins that are solid at 25° C., and even more preferably a bisphenol A-type epoxy resin that is solid at 25° C. Furthermore, from the viewpoint of the dispersion stability and various properties of the resulting resin composition, it is preferable to use, as component (A), an epoxy resin that is solid at 25° C. and has an epoxy equivalent of 500 g / eq. to 30,000 g / eq., more preferably an epoxy resin that is solid at 25° C. and has an epoxy equivalent of 1,000 g / eq. to 10,000 g / eq., and even more preferably an epoxy resin that is solid at 25° C. and has an epoxy equivalent of 1,500 g / eq. It is even more preferable to use an epoxy resin that is solid at 25°C and has an epoxy equivalent of 2,000 g / eq. to 6,000 g / eq., even more preferable to use an epoxy resin that is solid at 25°C and has an epoxy equivalent of 2,000 g / eq. to 5,000 g / eq., and particularly preferable to use an epoxy resin that is solid at 25°C and has an epoxy equivalent of 2,500 g / eq. to 3,500 g / eq.

[0048] When the resin composition of the present invention contains water, as component (B), from the viewpoint of the dispersion stability and various properties of the resulting resin composition, it is preferable to use one or more selected from the group consisting of polyether polyurethane prepolymers and polyether polyurethanes obtained by reacting raw materials containing one or more polyalkylene glycols, among the above-mentioned polyether polyurethane prepolymers and polyether polyurethanes, more preferably one or more selected from the group consisting of polyether polyurethane prepolymers and polyether polyurethanes obtained by reacting raw materials containing one or more selected from the group consisting of polyethylene glycol, polypropylene glycol, and polytetramethylene ether glycol, even more preferably one or more selected from the group consisting of polyether polyurethane prepolymers and polyether polyurethanes obtained by reacting raw materials containing one or more selected from the group consisting of polypropylene glycol and polytetramethylene ether glycol, and particularly preferably one or more selected from the group consisting of polyether polyurethane prepolymers and polyether polyurethanes obtained by reacting raw materials containing polytetramethylene ether glycol. From the viewpoint of the dispersion stability and various properties of the resulting resin composition, the acid value of the polyether polyurethane prepolymer and polyether polyurethane used is preferably 0 to 70 mgKOH / g, more preferably 10 to 60 mgKOH / g, even more preferably 15 to 50 mgKOH / g, and particularly preferably 20 to 40 mgKOH / g.

[0049] 1-4. Other Components In addition to the above-described components (A), (B), and water, the resin composition of the present invention may contain, depending on the purpose, a solvent, a neutralizing agent, a surfactant, an aminosilane compound, an amide compound, a carbodiimide compound, an isocyanate compound (excluding polyether polyurethane prepolymer), a polyetheramine compound, a phosphoric acid-modified epoxy resin, a melamine resin, a phenolic resin, or the like. The solvent that may be contained in the resin composition of the present invention is not particularly limited, and known solvents can be used. Examples of such solvents include acetone, methyl ethyl ketone, dioxane, tetrahydrofuran, N-methyl-2-pyrrolidone, ethylene glycol monomethyl ether, propylene glycol monomethyl ether, ethylene glycol monomethyl ether acetate, and propylene glycol monomethyl ether acetate. One or more of these solvents can be used. When the resin composition of the present invention contains a solvent, the content of the solvent is not particularly limited and can be adjusted appropriately depending on the purpose. For example, the solvent can be contained in an amount of 0.1 to 50 mass% based on the total amount of the resin composition. From the viewpoints of the adhesion and corrosion resistance of the resin composition to metals, reduction of the environmental load, and ease of handling of the resin composition, the upper limit of the solvent content is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less, based on the total amount of the resin composition. In the present invention, by containing the above-mentioned component (A) and component (B), a resin composition excellent in stability and ease of handling can be produced even when the solvent content is low or not contained.

[0050] The neutralizing agent that can be contained in the resin composition of the present invention is not particularly limited, and known neutralizing agents can be used. Examples of such neutralizing agents include trialkylamines such as trimethylamine, triethylamine, and tributylamine; N,N-dialkylalkanolamines such as N,N-dimethylethanolamine, N,N-dimethylpropanolamine, N,N-dipropylethanolamine, and 1-dimethylamino-2-methyl-2-propanol; tertiary amine compounds such as N-alkyl-N,N-dialkanolamines and trialkanolamines such as triethanolamine; ammonia, trimethylammonium hydroxide, sodium hydroxide, potassium hydroxide, and lithium hydroxide. One or more of these can be used. In the present invention, when one or more members selected from the group consisting of polyether polyurethane prepolymers having an acid value of 10 to 60 mgKOH / g and polyether polyurethanes having an acid value of 10 to 60 mgKOH / g are used as component (B), from the viewpoint of the stability and handleability of the resin composition, the resin composition preferably contains a neutralizing agent in an amount of 0.01 to 5 mass %, more preferably 0.05 to 3 mass %, based on the total amount of the resin composition.

[0051] The surfactant that can be contained in the resin composition of the present invention is not particularly limited, and known surfactants can be used. Examples of such surfactants include known anionic surfactants, nonionic surfactants, cationic surfactants, amphoteric surfactants, etc. One or more of these can be used.

[0052] Examples of anionic surfactants include alkyl sulfates such as sodium dodecyl sulfate, potassium dodecyl sulfate, and ammonium dodecyl sulfate; polyoxyethylene ether sulfates such as sodium dodecyl polyglycol ether sulfate and ammonium polyoxyethylene alkyl ether sulfate; ammonium salts of alkyl sulfonates such as the ammonium salt of sulfonated paraffin; fatty acid salts such as sodium laurate, triethanolamine oleate, and triethanolamine abietate; alkylaryl sulfonates such as sodium benzenesulfonate and the alkali metal sulfate of alkaliphenol hydroxyethylene; alkylnaphthalenesulfonate, naphthalenesulfonic acid-formalin condensates, dialkyl sulfosuccinates, polyoxyethylene alkyl sulfate salts, polyoxyethylene alkylaryl sulfate salts, polyoxyethylene ether phosphates, polyoxyethylene alkyl ether acetates, N-acylamino acid salts, and N-acylmethyl taurine salts. One or more of these may be used.

[0053] Examples of nonionic surfactants include fatty acid partial esters of polyhydric alcohols such as sorbitan monolaurate and sorbitan monooleate; polyoxyethylene glycol fatty acid esters; polyglycerin fatty acid esters; ethylene oxide and / or propylene oxide adducts of alcohols having 1 to 18 carbon atoms; ethylene oxide and / or propylene oxide adducts of alkylphenols; ethylene oxide and / or propylene oxide adducts of alkylene glycols and / or alkylenediamines, etc. Examples of alcohols having 1 to 18 carbon atoms that constitute nonionic surfactants include methanol, ethanol, propanol, 2-propanol, butanol, 2-butanol, tertiary butanol, amyl alcohol, isoamyl alcohol, tertiary amyl alcohol, hexanol, octanol, decane alcohol, lauryl alcohol, myristyl alcohol, palmityl alcohol, and stearyl alcohol. Examples of alkylphenols constituting the nonionic surfactant include phenol, methylphenol, 2,4-di-tert-butylphenol, 2,5-di-tert-butylphenol, 3,5-di-tert-butylphenol, 4-(1,3-tetramethylbutyl)phenol, 4-isooctylphenol, 4-nonylphenol, 4-tert-octylphenol, 4-dodecylphenol, 2-(3,5-dimethylheptyl)phenol, 4-(3,5-dimethylheptyl)phenol, naphthol, bisphenol A, and bisphenol F. Examples of alkylene glycols constituting the nonionic surfactant include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 2-methyl-1,3-propanediol, 2-butyl-2-ethyl-1,3-propanediol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, and 1,6-hexanediol. Examples of alkylene diamines include those in which the alcoholic hydroxyl groups of these alkylene glycols have been substituted with amino groups.Furthermore, the ethylene oxide and propylene oxide adducts may be random adducts or block adducts.

[0054] Examples of cationic surfactants include quaternary ammonium salts such as lauryltrimethylammonium chloride, stearyltrimethylammonium chloride, distearyldimethylammonium chloride, didecyldimethylammonium chloride, laurylbenzyldimethylammonium chloride, and didecyldimethylammonium chloride; alkylpyridinium bromide; and imidazolinium laurate. These may be used alone or in combination.

[0055] Examples of amphoteric surfactants include betaine-type amphoteric surfactants such as coconut oil fatty acid amidopropyl dimethyl acetate betaine, lauryl dimethyl amino acid betaine, 2-alkyl-N-carboxymethyl-N-hydroxymethyl imidazolinium betaine, lauryl hydroxysulfobetaine, lauroyl amidoethyl hydroxyethyl carboxymethyl betaine, and metal salts of hydroxypropyl phosphate; and amino acid-type, sulfate ester-type, and sulfonic acid-type amphoteric surfactants such as metal salts of β-lauryl aminopropionic acid. These may be used alone or in combination of two or more.

[0056] In the present invention, from the viewpoints of the adhesiveness and corrosion resistance of the resin composition to metals, the ease of handling of the resin composition, etc., it is preferable to contain one or more surfactants selected from the group consisting of anionic surfactants and nonionic surfactants, more preferably to contain at least one nonionic surfactant, and even more preferably to contain at least one nonionic surfactant having an alkylene oxide skeleton. Furthermore, among nonionic surfactants, it is preferable to contain a nonionic surfactant having a weight average molecular weight of 1,000 to 50,000, more preferably a nonionic surfactant having a weight average molecular weight of 5,000 to 30,000, even more preferably a nonionic surfactant having a weight average molecular weight of 10,000 to 20,000, and particularly preferably a nonionic surfactant having a weight average molecular weight of 14,000 to 18,000.

[0057] When the resin composition of the present invention contains a surfactant, the content of the surfactant in the resin composition is not particularly limited and can be appropriately adjusted depending on the purpose. From the viewpoints of the handleability of the resulting resin composition and the adhesion to metals and corrosion resistance, the content of the surfactant in the resin composition is preferably 0.01 to 20 mass%, more preferably 0.1 to 15 mass%, even more preferably 0.2 to 10 mass%, even more preferably 0.5 to 6 mass%, and particularly preferably 3.0 to 5.0 mass%, relative to the total amount of the resin composition.

[0058] The aminosilane compound that can be used in the present invention is not particularly limited as long as it contains an amino group and a silicon-containing group in the molecule, and known silane coupling agents can be used. Examples of such aminosilane compounds include 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-methyl-3-(trimethoxysilyl)propylamine, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropylmethyldimethoxysilane, and N-(6-aminohexyl)-3-aminopropyltriethoxysilane. -aminopropyltrimethoxysilane, 3-aminopropyldiethoxymethylsilane, 3-t-butylaminopropyltrimethoxysilane, 3-cyclohexylaminopropyltrimethoxysilane, N-methyl-3-amino-2-methylpropyltrimethoxysilane, N-ethyl-3-amino-2-methylpropylmethyldimethoxysilane, N-ethyl-3-amino-2-methylpropyltrimethoxysilane, N-ethyl-3-amino-2-methylpropyldiethoxymethylsilane, N-ethyl-3-amino-2-methylpropyldiethoxymethylsilane -amino-2-methylpropyltriethoxysilane, N-butyl-3-amino-2-methylpropyltrimethoxysilane, 3-(N-methyl-2-amino-1-methyl-1-ethoxy)propyltrimethoxysilane, N-ethyl-4-amino-3,3-dimethylbutyldimethoxymethylsilane, N-ethyl-4-amino-3,3-dimethylbutyltrimethoxysilane, bis-(3-trimethoxysilyl-2-methylpropyl)amine, N-(3-trimethoxysilylpropyl)-3-amino-2-methylpropyl trimethylpropyltrimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, 3-trimethoxysilylpropyl-3-[N-(3-trimethoxysilyl)-propylamino]-2-propionic acid methyl ester, 3-triethoxysilylpropyl-3-[N-(3-triethoxysilyl)-propylamino]-2-propionic acid methyl ester, 3-trimethoxysilylpropyl-3-[N-(3-triethoxysilyl)-propylamino]-2-propionic acid methyl ester, N-ethyl-4-amino-3,Examples of suitable silanes include 3-dimethylbutyldimethoxymethylsilane, N-ethyl-4-amino-3,3-dimethylbutyltrimethoxysilane, N-(3-trimethoxysilyl)propyl-3-[N-(3-trimethoxysilyl)propylamino]propionamide, N-(3-triethoxysilyl)propyl-3-[N-(3-triethoxysilyl)propylamino]propionamide, N-(3-trimethoxysilyl)propyl-3-[N-(3-triethoxysilyl)propylamino]propionamide, N,N-bis[(3-trimethoxysilyl)propyl]amine, N,N-bis[(3-triethoxysilyl)propyl]amine, N,N-bis[(3-tripropoxysilyl)propyl]amine, and N,N-bis[(3-trimethoxysilyl)-2-methylpropyl]amine. These may be used alone or in combination.

[0059] When the resin composition of the present invention contains an aminosilane compound, the content of the aminosilane compound in the resin composition is not particularly limited and can be appropriately adjusted depending on the purpose. From the viewpoint of the adhesion to metal and corrosion resistance of the resulting resin composition, the content of the aminosilane compound in the resin composition is preferably 0.01 to 20 mass%, more preferably 0.1 to 10 mass%, and even more preferably 0.2 to 5 mass%, relative to the total mass of the resin composition.

[0060] The amide compound that can be used in the present invention is not particularly limited as long as it has one or more amide groups in the molecule. Examples of such amide compounds include succinic acid dihydrazide, adipic acid dihydrazide, phthalic acid dihydrazide, isophthalic acid dihydrazide, terephthalic acid dihydrazide, p-oxybenzoic acid hydrazide, salicylic acid hydrazide, maleic acid dihydrazide, dicyandiamide, methylguanidine, ethylguanidine, propylguanidine, butylguanidine, dimethylguanidine, trimethylguanidine, phenylguanidine, and diphenylguanidine. One or more of these compounds can be used.

[0061] When the resin composition of the present invention contains an amide compound, the content of the amide compound in the resin composition is not particularly limited and can be appropriately adjusted depending on the purpose. From the viewpoint of the adhesion to metal and corrosion resistance of the resulting resin composition, the content of the amide compound in the resin composition is preferably 0.01 to 20 mass%, more preferably 0.1 to 10 mass%, and even more preferably 0.2 to 5 mass%, relative to the total mass of the resin composition.

[0062] The carbodiimide compound that can be used in the present invention is not particularly limited as long as it has one or more carbodiimide groups (-N=C=N-) in the molecule. Examples of such carbodiimide compounds include N,N'-dicyclohexylcarbodiimide, N,N'-dimethylcarbodiimide, N,N'-diisopropylcarbodiimide, N,N'-diisobutylcarbodiimide, N,N'-dioctylcarbodiimide, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide, N,N'-bis(2,6-diisopropylphenyl)carbodiimide, poly(1,6-hexamethylenecarbodiimide), and the like. Examples of the carbodiimide that can be used include poly(4,4'-methylenebiscyclohexylcarbodiimide), poly(1,3-cyclohexylenecarbodiimide), poly(1,4-cyclohexylenecarbodiimide), and poly(4,4'-dicyclohexylmethanecarbodiimide). Commercially available products such as Carbodilite V-02, V-02-L2, SV-02, V-04, V-10, E-02, E-03A, and E-05 (all manufactured by Nisshinbo Chemical Inc.) can also be used. In the present invention, among these, from the viewpoint of the adhesion to metal and corrosion resistance of the resulting resin composition, it is preferable to use a carbodiimide compound having a carbodiimide equivalent of 100 to 800 g / eq., and a carbodiimide compound having a carbodiimide equivalent of 200 to 700 g / eq. It is more preferable to use a carbodiimide compound having a carbodiimide equivalent of 300 to 600 g / eq., even more preferable to use a carbodiimide compound having a carbodiimide equivalent of 400 to 500 g / eq.

[0063] When the resin composition of the present invention contains a carbodiimide compound, the content of the carbodiimide compound in the resin composition is not particularly limited and can be appropriately adjusted depending on the purpose. From the viewpoint of the adhesion to metal and corrosion resistance of the resulting resin composition, the content of the carbodiimide compound in the resin composition is preferably 0.01 to 20 mass%, more preferably 0.1 to 10 mass%, and even more preferably 0.2 to 5 mass%, based on the total amount of the resin composition.

[0064] The isocyanate compound that can be used in the present invention is not particularly limited as long as it has one or more isocyanate groups in the molecule. From the viewpoint of the adhesion to metals and corrosion resistance of the resulting resin composition, an isocyanate compound having two isocyanate groups in the molecule is preferred. Examples of such isocyanate compounds include aliphatic diisocyanates such as hexamethylene diisocyanate and 2,2,4-trimethylhexamethylene diisocyanate, alicyclic diisocyanates such as isophorone diisocyanate, 4,4-dicyclohexylmethane diisocyanate and 1,3-bis(isocyanatomethyl)cyclohexane, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, 1,5-naphthylene diisocyanate, and 1,4-naphthylene diisocyanate. Examples of the diisocyanate include aromatic diisocyanates such as methyl anate, phenylene diisocyanate, tetramethylxylylene diisocyanate, 4,4'-diphenylether diisocyanate, 2-nitrodiphenyl-4,4'-diisocyanate, 2,2'-diphenylpropane-4,4'-diisocyanate, 3,3'-dimethyldiphenylmethane-4,4'-diisocyanate, 4,4'-diphenylpropane diisocyanate, 3,3'-dimethoxydiphenyl-4,4'-diisocyanate, and xylylene diisocyanate. Polymers, adducts, biuret forms, nurate forms, and blocked forms blocked with a blocking agent may also be used.In this case, examples of the blocking agent include phenol-based blocking agents such as phenol, cresol, xylenol, chlorophenol, and ethylphenol; lactam-based blocking agents such as ε-caprolactam, δ-valerolactam, γ-butyrolactam, and β-propiolactam; active methylene-based blocking agents such as ethyl acetoacetate and acetylacetone; methanol, ethanol, propanol, butanol, amyl alcohol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, propylene glycol monomethyl ether, benzyl ether, methyl glycolate, butyl glycolate, diacetone alcohol, methyl lactate, and lactic acid. oxime-based blocking agents such as formaldehyde oxime, acetaldoxime, acetoxime, methyl ethyl ketoxime, diacetyl monooxime, and cyclohexane oxime; mercaptan-based blocking agents such as butyl mercaptan, hexyl mercaptan, t-butyl mercaptan, thiophenol, methylthiophenol, and ethylthiophenol; acid amide-based blocking agents such as acetic acid amide and benzamide; imide-based blocking agents such as succinimide and maleic acid imide; amine-based blocking agents such as xylidine, aniline, butylamine, and dibutylamine; imidazole-based blocking agents such as imidazole and 2-ethylimidazole; and imine-based blocking agents such as methyleneimine and propyleneimine.

[0065] When the resin composition of the present invention contains an isocyanate compound, the content of the isocyanate compound in the resin composition is not particularly limited and can be appropriately adjusted depending on the purpose. From the viewpoint of the adhesion to metal and corrosion resistance of the resulting resin composition, the content of the isocyanate compound in the resin composition is preferably 0.01 to 20 mass%, more preferably 0.1 to 10 mass%, and even more preferably 0.2 to 5 mass%, based on the total amount of the resin composition.

[0066] The polyetheramine compounds that can be used in the present invention are not particularly limited as long as they contain a polyether group consisting of a polyoxyalkylene structure such as a polyoxyethylene group, a polyoxypropylene group, or a polyoxybutylene group in the molecule, and at least one amino group. In this case, the polyetheramine compound may contain only polyoxyethylene groups, only polyoxypropylene groups, or only polyoxybutylene groups as the polyether groups in the molecule, or may contain two or more groups selected from the group consisting of polyoxyethylene groups, polyoxypropylene groups, and polyoxybutylene groups. The number of repeating oxyalkylene structures in the polyether group is not particularly limited and can be adjusted depending on the purpose. For example, the number of repeating oxyalkylene structures in the polyetheramine compound can be 2 to 500, calculated as the total number of repeating oxyalkylene groups of one or more types. Examples of such polyetheramine compounds include polyethylene glycol amine, polyethylene glycol diamine, methoxypolyethylene glycol amine, polypropylene glycol amine, polypropylene glycol diamine, methoxypolypropylene glycol amine, polybutylene glycol amine, polybutylene glycol diamine, methoxypolybutylene glycol amine, polyoxyethylene polyoxypropylene amine, polyoxyethylene polyoxypropylene diamine, and methoxypolyoxyethylene polyoxypropylene amine. Furthermore, commercially available products can also be used as the polyetheramine compound, and examples of commercially available products include JEFFAMINE (registered trademark) M Series (M-600, M-1000, M-2005, M-2070), JEFFAMINE D Series (D-230, D-400, D-2000, D-4000), JEFFAMINE ED Series (ED-600, ED-900, ED-2003), and JEFFAMINE T Series (T-403, T-3000, T-5000) (all manufactured by HUNTSMAN).

[0067] In the present invention, among these, from the viewpoint of the adhesion to metals and corrosion resistance of the resulting resin composition, it is preferable to use a polyetheramine compound having a polyether group, an amino group, and a methoxy group in the molecule as the polyetheramine compound, and it is also preferable to use a polyetheramine compound having only polyoxyethylene groups, only polyoxypropylene groups, or polyoxyethylene and polyoxypropylene groups as the polyether group. More specifically, in the present invention, it is particularly preferable to use a methoxypolyoxyethylenepolyoxypropyleneamine compound having 1 to 100 repeating oxyethylene groups and 2 to 50 repeating oxypropylene groups in the molecule as the polyetheramine compound.

[0068] When the resin composition of the present invention contains a polyetheramine-based compound, the content of the polyetheramine-based compound in the resin composition is not particularly limited and can be appropriately adjusted depending on the purpose. From the viewpoint of the adhesion to metal and corrosion resistance of the resulting resin composition, the content of the polyetheramine-based compound in the resin composition is preferably 0.01 to 20 mass%, more preferably 0.1 to 10 mass%, and even more preferably 0.2 to 5 mass%, based on the total amount of the resin composition.

[0069] The phosphoric acid-modified epoxy resin that can be used in the present invention is not particularly limited as long as it is a modified product obtained by reacting a phosphoric acid with an epoxy compound. Examples of such phosphoric acids that can be used include orthophosphoric acid, phosphorous acid, hypophosphorous acid, phosphonic acid, pyrophosphoric acid, and polyphosphoric acid such as triphosphoric acid. In this case, the epoxy compound that can be used is not particularly limited as long as it has at least one epoxy group in the molecule, and examples thereof include n-butyl glycidyl ether, C 12 ~C 14compounds having one epoxy group in the molecule, such as alkyl glycidyl ethers of the above alkyl glycidyl ethers, allyl glycidyl ether, 2-ethylhexyl glycidyl ether, styrene oxide, phenyl glycidyl ether, cresyl glycidyl ether, p-sec-butylphenyl glycidyl ether, t-butylphenyl glycidyl ether, glycidyl methacrylate, and tertiary carboxylic acid glycidyl esters; compounds having two epoxy groups in the molecule, such as ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, and neopentyl glycol diglycidyl ether; compounds having three epoxy groups in the molecule, such as trimethylolpropane triglycidyl ether and glycerin triglycidyl ether; bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol Examples of epoxy resins include phenol S-type epoxy resins, bisphenol AD-type epoxy resins, resorcinol-type epoxy resins, hydroquinone-type epoxy resins, catechol-type epoxy resins, dihydroxynaphthalene-type epoxy resins, biphenyl-type epoxy resins, tetramethylbiphenyl-type epoxy resins, oxazolidone ring-type epoxy resins, phenol novolac-type epoxy resins, cresol novolac-type epoxy resins, triphenylmethane-type epoxy resins, tetraphenylethane-type epoxy resins, dicyclopentadiene-phenol addition reaction-type epoxy resins, phenol aralkyl-type epoxy resins, naphthol novolac-type epoxy resins, naphthol aralkyl-type epoxy resins, naphthol-phenol co-condensed novolac-type epoxy resins, naphthol-cresol co-condensed novolac-type epoxy resins, aromatic hydrocarbon formaldehyde resin-modified phenolic resin-type epoxy resins, and biphenyl-modified novolac-type epoxy resins. One or more of these may be used.

[0070] The phosphoric acid-modified epoxy resin that can be used in the present invention can be obtained by reacting the above-mentioned epoxy compound with a phosphoric acid at an equivalent ratio of 1:0.1 to 1:5, for example, at room temperature to 100° C. In this case, from the viewpoint of the adhesion to metal and corrosion resistance of the resulting resin composition, the phosphoric acid-modified epoxy resin is preferably a phosphoric acid-modified epoxy resin obtained by reacting one or more epoxy compounds selected from the group consisting of bisphenol A epoxy resins, bisphenol F epoxy resins, bisphenol S epoxy resins, and bisphenol AD ​​epoxy resins with a phosphoric acid compound such as orthophosphoric acid, metaphosphoric acid, phosphonic acid, pyrophosphoric acid, or polyphosphoric acid at an equivalent ratio of 1:0.5 to 1:3, and more preferably a phosphoric acid-modified epoxy resin obtained by reacting at an equivalent ratio of 1:1 to 1:2.

[0071] When the resin composition of the present invention contains a phosphoric acid-modified epoxy resin, the content of the phosphoric acid-modified epoxy resin in the resin composition is not particularly limited and can be appropriately adjusted depending on the purpose. From the viewpoint of the adhesion to metal and corrosion resistance of the resulting resin composition, the content of the phosphoric acid-modified epoxy resin in the resin composition is preferably 0.01 to 20 mass%, more preferably 0.1 to 10 mass%, and even more preferably 0.2 to 5 mass%, based on the total amount of the resin composition.

[0072] The melamine resin that can be used in the present invention is not particularly limited as long as it is a known melamine resin. Examples of such melamine resins include partially or fully methylolated melamine obtained by reacting melamine with formaldehyde, alkyl ether-type melamine resins obtained by partially or fully etherifying the methylol groups of methylolated melamine resins with alcohol, imino group-containing melamine resins, and mixtures thereof. One or more of these can be used. In the present invention, among these, it is preferable to use an imino group-containing melamine resin as the melamine resin from the viewpoint of the adhesion to metal and corrosion resistance of the resulting resin composition. Furthermore, commercially available melamine resins can also be used in the present invention, such as the CYMEL (registered trademark) series of melamine resins (manufactured by Allnex).

[0073] When the resin composition of the present invention contains a melamine resin, the content of the melamine resin in the resin composition is not particularly limited and can be appropriately adjusted depending on the purpose. From the viewpoint of the adhesion to metal and corrosion resistance of the resulting resin composition, the content of the melamine resin in the resin composition is preferably 0.01 to 20 mass%, more preferably 0.1 to 10 mass%, and even more preferably 0.2 to 5 mass%, based on the total amount of the resin composition.

[0074] The phenolic resin that can be used in the present invention is not particularly limited as long as it is a known phenolic resin. Examples of such phenolic resins include bisphenol A phenolic resins, bisphenol E phenolic resins, bisphenol F phenolic resins, bisphenol S phenolic resins, phenol novolac resins, bisphenol A novolac phenolic resins, glycidyl ester phenolic resins, aralkyl novolac phenolic resins, biphenyl aralkyl phenolic resins, resol phenolic resins, cresol novolac phenolic resins, multifunctional phenolic resins, naphthol resins, naphthol novolac resins, multifunctional naphthol resins, anthracene phenolic resins, naphthalene skeleton-modified novolac phenolic resins, phenol aralkyl phenolic resins, naphthol aralkyl phenolic resins, dicyclopentadiene phenolic resins, biphenyl phenolic resins, alicyclic phenolic resins, polyol phenolic resins, phosphorus-containing phenolic resins, polymerizable unsaturated hydrocarbon group-containing phenolic resins, and hydroxyl group-containing silicone resins. These resins may be used alone or in combination. In the present invention, among these, it is preferable to use a resol-type phenolic resin as the phenolic resin from the viewpoint of the adhesion to metals and corrosion resistance of the resulting resin composition. Furthermore, as the phenolic resin that can be used in the present invention, a commercially available product can be used, for example, a series of phenolic resins under the name SUMILITE RESIN (registered trademark) (manufactured by Sumitomo Bakelite Co., Ltd.).

[0075] When the resin composition of the present invention contains a phenolic resin, the content of the phenolic resin in the resin composition is not particularly limited and can be appropriately adjusted depending on the purpose. From the viewpoint of the adhesion to metal and corrosion resistance of the resulting resin composition, the content of the phenolic resin in the resin composition is preferably 0.01 to 20 mass %, more preferably 0.1 to 10 mass %, and even more preferably 0.2 to 5 mass %, based on the total amount of the resin composition.

[0076] The resin composition of the present invention contains components such as polyether polyurethane prepolymer and polyether polyurethane, which have a polyether urethane main skeleton and thereby provide excellent flexibility in the polymer chain, and is therefore believed to have excellent adhesive properties, particularly excellent adhesive properties in a short period of time.Furthermore, the resin composition of the present invention contains an epoxy resin that is solid at 25°C, which improves the stability and coatability of the resin composition, and is therefore believed to have excellent adhesive properties, particularly excellent adhesive properties in a short period of time and corrosion resistance.

[0077] 1-5. Manufacturing Method of Resin Composition The method for manufacturing the resin composition of the present invention is not particularly limited, and it can be manufactured by, for example, a method of mixing component (A) consisting of an epoxy resin that is solid at 25°C with component (B) consisting of one or more selected from the group consisting of polyether polyurethane prepolymers and polyether polyurethanes by a known method. Here, component (A) consisting of an epoxy resin that is solid at 25°C may be used in its solid form, in a state dispersed in water, or in a state dissolved in a solvent. From the viewpoint of easily manufacturing a resin composition that is excellent in stability and handleability, it is preferable to manufacture the resin composition using an aqueous dispersion emulsion in which component (A) consisting of an epoxy resin that is solid at 25°C is dispersed in a solvent containing water. Here, the method for dispersing component (A) consisting of an epoxy resin that is solid at 25°C in water is not particularly limited, and for example, a method of forcibly emulsifying an epoxy resin in water using a surfactant, a method of dispersing a self-emulsifying epoxy resin in water, or the like can be used.

[0078] In the present invention, the surfactant that can be used when producing a resin composition using an aqueous emulsion obtained by dispersing component (A) consisting of an epoxy resin that is solid at 25° C. in a solvent containing water is not particularly limited, and the above-mentioned known anionic surfactants, nonionic surfactants, cationic surfactants, amphoteric surfactants, etc. can be used. From the viewpoints of the adhesion to metal, corrosion resistance, handleability, etc. of the resulting resin composition, it is preferable to contain one or more surfactants selected from the group consisting of anionic surfactants and nonionic surfactants, it is more preferable to contain at least one nonionic surfactant, and it is even more preferable to contain at least one nonionic surfactant having an alkylene oxide skeleton. In this case, among the nonionic surfactants, from the viewpoints of the adhesion to metals, corrosion resistance, handleability, etc. of the resulting resin composition, it is preferable to contain a nonionic surfactant having a weight average molecular weight of 1,000 to 50,000, more preferably a nonionic surfactant having a weight average molecular weight of 5,000 to 30,000, even more preferably a nonionic surfactant having a weight average molecular weight of 10,000 to 20,000, and particularly preferably a nonionic surfactant having a weight average molecular weight of 14,000 to 18,000. Furthermore, the content of the surfactant in the water-dispersed emulsion obtained by dispersing component (A) consisting of an epoxy resin that is solid at 25°C in a solvent containing water is not particularly limited, but can be, for example, 0.01 to 20 mass%. From the viewpoints of the adhesiveness to metals, corrosion resistance, handleability, etc. of the resulting resin composition, the content of the surfactant is preferably 0.1 to 20 mass %, more preferably 0.5 to 10 mass %, even more preferably 0.5 to 8.0 mass %, and particularly preferably 3.0 to 6.0 mass %, relative to the total amount of the water-dispersed emulsion obtained by dispersing component (A), which is an epoxy resin that is solid at 25°C, in a solvent containing water.

[0079] Furthermore, when producing the resin composition of the present invention, the polyether polyurethane prepolymer may be used as a solid or liquid polyether polyurethane prepolymer alone, in a water-dispersed state, or dissolved in a solvent. From the viewpoint of easily producing a resin composition with excellent stability and ease of handling, it is preferable to produce the resin composition using an aqueous emulsion in which the polyether polyurethane prepolymer is dispersed in a solvent containing water. In this case, the method for dispersing the polyether polyurethane prepolymer in water is not particularly limited. For example, a method of forcibly emulsifying the polyether polyurethane prepolymer in water using a surfactant, or a method of dispersing a self-emulsifying polyether polyurethane prepolymer in water can be used. The surfactant that can be used in this case is not particularly limited. The known anionic surfactants, nonionic surfactants, cationic surfactants, amphoteric surfactants, etc., described above can be used, and the content thereof is also not particularly limited. The content of the surfactant is, for example, preferably 0.1 to 20 mass %, more preferably 0.5 to 10 mass %, even more preferably 0.5 to 8.0 mass %, and particularly preferably 3.0 to 6.0 mass %, relative to the total amount of the water-dispersed emulsion in which a polyether polyurethane prepolymer is dispersed in a solvent containing water.

[0080] Furthermore, when producing the resin composition of the present invention, the polyether polyurethane may be used as a solid or liquid polyether polyurethane alone, in a water-dispersed state, or dissolved in a solvent. From the viewpoint of easily producing a resin composition with excellent stability and ease of handling, it is preferable to produce the resin composition using an aqueous emulsion in which the polyether polyurethane is dispersed in a solvent containing water. The method for dispersing the polyether polyurethane in water is not particularly limited. For example, a method of forcibly emulsifying the polyether polyurethane in water using a surfactant, or a method of dispersing a self-emulsifying polyether polyurethane in water can be used. The surfactant that can be used is not particularly limited. Examples of the known anionic surfactants, nonionic surfactants, cationic surfactants, and amphoteric surfactants mentioned above can be used. The surfactant content is also not particularly limited. For example, the surfactant content is preferably 0.1 to 20% by mass, more preferably 0.5 to 10% by mass, even more preferably 0.5 to 8.0% by mass, and particularly preferably 3.0 to 6.0% by mass, based on the total amount of the aqueous emulsion in which the polyether polyurethane is dispersed in a solvent containing water.

[0081] In the present invention, from the viewpoint of more easily obtaining an aqueous resin composition having excellent adhesive properties, particularly adhesive properties that allow bonding by pressure bonding in a short time, and corrosion resistance, it is particularly preferred to produce the resin composition by mixing an aqueous dispersion emulsion of component (A) consisting of an epoxy resin that is solid at 25°C with an aqueous dispersion emulsion of component (B) consisting of one or more members selected from the group consisting of polyether polyurethane prepolymers and polyether polyurethanes.

[0082] 1-6. Uses of Resin Composition The resin composition of the present invention can be used for any application that uses an epoxy resin or a urethane resin, without any particular limitation. The resin composition of the present invention can be used, for example, as an adhesive, coating, sealant, etc. for substrates such as metal, wood, glass, concrete, plastic, and ceramic. More specifically, it can be used as an adhesive or coating for bonding various substrates in the fields of automobiles, vehicles (bullet trains, electric trains, etc.), civil engineering, architecture, ships, airplanes, and the aerospace industry, as well as an adhesive or sealant for general office materials, medical materials, and electronic materials. Among these, the resin composition of the present invention contains the above-mentioned specific components (A) and (B), and therefore has excellent adhesion, particularly to metals. Therefore, it is preferably used as a resin composition for metal surface treatment, such as an adhesive between metal substrates or between metal substrates and other substrates, or a coating agent for metal substrates.

[0083] 2. Metal Surface Treatment Resin Composition The metal surface treatment resin composition of the present invention contains component (A) consisting of an epoxy resin that is solid at 25°C and component (B) consisting of one or more species selected from the group consisting of polyether polyurethane prepolymers and polyether polyurethanes. The components described above can be used as component (A) consisting of an epoxy resin that is solid at 25°C and component (B) consisting of one or more species selected from the group consisting of polyether polyurethane prepolymers and polyether polyurethanes. The content of component (A) consisting of an epoxy resin that is solid at 25°C in the metal surface treatment resin composition of the present invention is not particularly limited and can be adjusted appropriately depending on the purpose. From the viewpoint of improving the adhesion and corrosion resistance of the metal surface treatment resin composition, particularly the adhesion upon short-term pressure bonding, the content of component (A) in the metal surface treatment resin composition is preferably 3 to 60 mass %, more preferably 5 to 50 mass %, even more preferably 8 to 45 mass %, and even more preferably 20 to 40 mass %, based on the total amount of the metal surface treatment resin composition.

[0084] The content of component (B), which is one or more selected from the group consisting of polyether polyurethane prepolymers and polyether polyurethanes, in the metal surface treatment resin composition of the present invention is not particularly limited and can be appropriately adjusted depending on the purpose. From the viewpoint of improving the adhesiveness and corrosion resistance of the metal surface treatment resin composition, particularly the adhesiveness after short-term pressure bonding, the content of component (B) is preferably 1 to 50 mass %, more preferably 2 to 40 mass %, even more preferably 3 to 30 mass %, and particularly preferably 4 to 10 mass %, based on the total amount of the metal surface treatment resin composition.

[0085] The content ratio of component (A) consisting of an epoxy resin that is solid at 25°C to component (B) consisting of one or more selected from the group consisting of polyether polyurethane prepolymers and polyether polyurethanes in the metal surface treatment resin composition of the present invention is not particularly limited and can be adjusted depending on the purpose. From the viewpoint of improving the adhesion and corrosion resistance of the metal surface treatment resin composition, particularly the adhesion after short-term pressure bonding, the content ratio of component (A) to component (B) in the metal surface treatment resin composition is preferably 5:95 to 98:2 by mass, more preferably 20:80 to 95:5, even more preferably 50:50 to 92:8, and particularly preferably 70:30 to 90:10.

[0086] The water content in the metal surface treatment resin composition of the present invention is not particularly limited and can be adjusted as appropriate. From the viewpoints of adhesion and corrosion resistance of the metal surface treatment resin composition to metals, reduction of environmental impact, and ease of handling of the metal surface treatment resin composition, the water content is preferably 10 to 90 mass%, more preferably 20 to 80 mass%, even more preferably 30 to 70 mass%, and particularly preferably 40 to 60 mass%, based on the total amount of the metal surface treatment resin composition. In this case, tap water, ion-exchanged water, distilled water, natural water, pure water, etc. can be used as the water, depending on the purpose.

[0087] When the metal surface treatment resin composition of the present invention contains water, the ratio of the contents of component (A), component (B), and water is not particularly limited and can be adjusted depending on the purpose. From the viewpoints of adhesion and corrosion resistance of the metal surface treatment resin composition, reduction of environmental load, and ease of handling of the metal surface treatment resin composition, the ratio of the contents of component (A), component (B), and water in the metal surface treatment resin composition, when the sum of the contents of component (A), component (B), and water is taken as 100, is preferably 3 to 80:1 to 60:10 to 90, more preferably 5 to 60:2 to 50:20 to 80, even more preferably 8 to 50:3 to 40:30 to 70, and particularly preferably 20 to 40:4 to 10:40 to 60. The resin composition for metal surface treatment of the present invention contains the above-mentioned specific component (A), component (B), and water in such a content ratio, so that a water-dispersed emulsion having excellent dispersion stability as a resin composition for metal surface treatment can be obtained, and therefore a resin composition for metal surface treatment having reduced environmental impact and excellent handleability can be obtained.

[0088] When the metal surface treatment resin composition of the present invention contains water, it is preferable to use, as component (A), a bisphenol type epoxy resin that is solid at 25° C. among the above-mentioned epoxy resins that are solid at 25° C., from the viewpoint of the dispersion stability and various properties of the resulting metal surface treatment resin composition, and it is more preferable to use one or more selected from the group consisting of bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, and bisphenol AD ​​type epoxy resins that are solid at 25° C., and it is even more preferable to use a bisphenol A type epoxy resin that is solid at 25° C. Furthermore, from the viewpoint of the dispersion stability and various properties of the resulting metal surface treatment resin composition, it is preferable to use, as component (A), an epoxy resin that is solid at 25° C. and has an epoxy equivalent of 500 g / eq. to 30,000 g / eq., and an epoxy equivalent of 1,000 g / eq. to 10,000 g / eq. It is more preferable to use an epoxy resin that is solid at 25°C and has an epoxy equivalent of 1,500 g / eq. to 6,000 g / eq., even more preferable to use an epoxy resin that is solid at 25°C and has an epoxy equivalent of 2,000 g / eq. to 5,000 g / eq., and particularly preferable to use an epoxy resin that is solid at 25°C and has an epoxy equivalent of 2,500 g / eq. to 3,500 g / eq.

[0089] When the metal surface treatment resin composition of the present invention contains water, as component (B), from the viewpoint of the dispersion stability and various properties of the resulting metal surface treatment resin composition, it is preferable to use, among the above-mentioned polyether polyurethane prepolymers and polyether polyurethanes, one or more selected from the group consisting of polyether polyurethane prepolymers and polyether polyurethanes obtained by reacting raw materials containing one or more polyalkylene glycols; it is more preferable to use one or more selected from the group consisting of polyether polyurethane prepolymers and polyether polyurethanes obtained by reacting raw materials containing one or more selected from the group consisting of polyethylene glycol, polypropylene glycol, and polytetramethylene ether glycol; it is even more preferable to use one or more selected from the group consisting of polyether polyurethane prepolymers and polyether polyurethanes obtained by reacting raw materials containing one or more selected from the group consisting of polypropylene glycol and polytetramethylene ether glycol; and it is particularly preferable to use one or more selected from the group consisting of polyether polyurethane prepolymers and polyether polyurethanes obtained by reacting raw materials containing polytetramethylene ether glycol. From the viewpoint of the dispersion stability and various properties of the resulting resin composition for metal surface treatment, the acid value of each of the polyether polyurethane prepolymer and polyether polyurethane used is preferably 0 to 70 mgKOH / g, more preferably 10 to 60 mgKOH / g, even more preferably 15 to 50 mgKOH / g, and particularly preferably 20 to 40 mgKOH / g.

[0090] In addition to the above-described components (A), (B), and water, the metal surface treatment resin composition of the present invention may contain other components such as surfactants, fillers, catalysts, lubricants, pigments, dyes, colorants, extenders, anticorrosives, flow modifiers, thixotropic agents, dispersants, antioxidants, adhesion promoters, and light stabilizers, depending on the intended purpose. In this case, examples of surfactants that may be contained in the metal surface treatment resin composition of the present invention include the above-described anionic surfactants, nonionic surfactants, cationic surfactants, and amphoteric surfactants. One or more of these surfactants may be used. When the metal surface treatment resin composition of the present invention contains a surfactant, the content of the surfactant in the metal surface treatment resin composition is not particularly limited and can be adjusted appropriately depending on the intended purpose. From the viewpoints of the handleability of the resulting resin composition for metal surface treatment and the adhesion to metal and corrosion resistance, the content of the surfactant in the resin composition for metal surface treatment is preferably 0.01 to 20 mass%, more preferably 0.1 to 15 mass%, even more preferably 0.2 to 10 mass%, even more preferably 0.5 to 6 mass%, and particularly preferably 3.0 to 5.0 mass%, relative to the total amount of the resin composition for metal surface treatment.

[0091] The metal material to be treated with the metal surface treatment resin composition of the present invention is not particularly limited, and examples thereof include copper, aluminum, gold, silver, iron, platinum, chromium, nickel, tin, titanium, zinc, manganese, magnesium, molybdenum, cobalt, tungsten, zirconium, lead, gallium, indium, and composite materials thereof. Metal oxides include single oxides and / or composite oxides of these metals. The metal surface treatment resin composition of the present invention can be applied to metal surfaces that have been processed into plates, foils, or the like and, if necessary, plated. The metal surface treatment resin composition of the present invention can also be used as an adhesive between metal substrates made of such metal materials, or between metal substrates and other substrates, or as a coating agent for metal substrates.

[0092] The method for applying the metal surface treatment resin composition of the present invention to a metal surface is not particularly limited, and known methods can be used. For example, the metal surface treatment resin composition of the present invention can be applied to a metal surface using spray coating, dip coating, roll coating, curtain coating, spin coating, or a combination of these methods. The temperatures of the metal surface and the metal surface treatment resin composition during application are also not particularly limited and can be adjusted according to the purpose. The temperatures of the metal surface and the metal surface treatment resin composition during application can be, for example, 10°C to 90°C. Furthermore, the drying method after application of the metal surface treatment resin composition to the metal surface is not particularly limited, and known methods can be used. Examples of such drying methods include using a drying oven, an electromagnetic induction heating oven, or the like, with a maximum temperature of 40°C to 250°C. Furthermore, as a method for using the metal surface treatment resin composition of the present invention as an adhesive between metal substrates or between a metal substrate and another substrate, for example, a method can be used in which the metal surface treatment resin composition is applied to a metal substrate by the method described above, and then dried as necessary, and then another substrate is laminated on the coating film of the metal surface treatment resin composition on the surface of the metal substrate, and the laminate is pressed and bonded by applying a pressure of 0.1 MPa to 100 MPa to the laminate while heating to a maximum temperature of 40°C to 250°C using a press, drying furnace, electromagnetic induction heating furnace, or the like as necessary.

[0093] 3. Manufacturing Method of Metal Laminate Plate The manufacturing method of the metal laminate plate of the present invention is a manufacturing method of a metal laminate plate including a step of applying the above-described resin composition to the surface of a first metal plate to form a coating film, and a step of laminating a second metal plate onto the coating film of the first metal plate to form a metal laminate. By using the manufacturing method of the metal laminate plate of the present invention, a metal laminate plate in which the metal plates are strongly bonded to each other can be obtained. In the present invention, the material of the metal plates used as the first metal plate and the second metal plate is not particularly limited. Examples of such materials include metal plates and steel plates containing copper, aluminum, gold, silver, iron, platinum, chromium, nickel, tin, titanium, zinc, manganese, magnesium, molybdenum, cobalt, tungsten, zirconium, lead, gallium, indium, and alloys thereof as the main component, and which may further contain optional components such as carbon, silicon, nitrogen, phosphorus, sulfur, boron, niobium, tantalum, vanadium, antimony, and germanium. Furthermore, the thickness of the metal plate used in the present invention is not particularly limited and can be adjusted appropriately depending on the purpose. For example, a metal plate having a thickness of 1 μm to 100 cm can be used. In the present invention, a metal laminate plate may be manufactured using two metal plates, or three or more metal plates. The multiple metal plates may be metal plates made of the same material and thickness, or may be metal plates made of different materials and thicknesses.

[0094] In the method for producing a metal laminate of the present invention, the method for applying the resin composition to the surface of the metal sheet is not particularly limited, and known methods can be used. For example, the resin composition can be applied to the surface of the metal sheet by spray coating, dip coating, roll coating, curtain coating, spin coating, or a combination thereof. The amount of the resin composition applied to the surface of the metal sheet is not particularly limited, and can be adjusted appropriately depending on the purpose. For example, the resin composition can be applied to the surface of the metal sheet in an amount such that the thickness of the coating film obtained by applying and drying the resin composition is 0.1 μm to 10 mm.

[0095] The method for producing a metal laminate of the present invention may comprise the steps of applying the above-described resin composition to the surface of a first metal sheet to form a coating film, and laminating a second metal sheet on the coating film on the surface of the first metal sheet to form a metal laminate, and may further comprise the steps of heating the metal laminate and crimping the metal laminate depending on the purpose. In the present invention, from the viewpoint of obtaining a more strongly bonded metal laminate, particularly a metal laminate that is strongly bonded in a short time, it is preferable to use a method for producing a metal laminate that includes the steps of applying the resin composition to the surface of the first metal sheet to form a coating film, laminating a second metal sheet on the coating film of the first metal sheet to form a metal laminate, and crimping the metal laminate.

[0096] The heating method in the step of heating the metal laminate that can be included in the method for producing a metal laminate of the present invention is not particularly limited, and known methods and conditions can be used. Examples of such heating methods include a method of heating the metal laminate to 40°C to 250°C using a drying oven, an electromagnetic induction heating oven, or the like. Furthermore, the pressure-bonding method in the step of pressure-bonding the metal laminate that can be included in the method for producing a metal laminate of the present invention is not particularly limited, and known methods can be used. Examples of such pressure-bonding methods include a method of compressing the metal laminate at a pressure of 0.1 MPa to 100 MPa using a press or the like. In the present invention, the step of heating the metal laminate and the step of pressure-bonding the metal laminate may be carried out simultaneously. Examples of such a method include a method in which the metal laminate is pressurized at a pressure of 0.1 MPa to 100 MPa using a press or the like in an environment of 40°C to 250°C using a drying furnace, an electromagnetic induction heating furnace, or the like, or a method in which the metal laminate is pressurized at a pressure of 0.1 MPa to 100 MPa using a heater press or the like heated to 40°C to 250°C to be pressure-bonded.

[0097] When the method for producing the metal laminate of the present invention includes a step of applying a resin composition to the surface of a first metal sheet to form a coating film, a step of laminating a second metal sheet on the coating film of the first metal sheet to form a metal laminate, and a step of crimping the metal laminate, the material and thickness of the metal sheet used are not particularly limited, and for example, metal sheets made of the material and thickness described above can be used. The first metal sheet and the second metal sheet may be metal sheets made of the same material and thickness, or may be metal sheets made of different materials and thicknesses. Furthermore, when the method for producing the metal laminate of the present invention includes a step of applying a resin composition to the surface of a first metal sheet to form a coating film, a step of laminating a second metal sheet on the coating film of the first metal sheet to form a metal laminate, and a step of crimping the metal laminate, the method for applying the resin composition to the metal sheet surface and the amount of resin composition applied to the metal sheet surface are not particularly limited, and can be, for example, the method and amount described above, respectively.

[0098] Furthermore, when the method for producing a metal laminate of the present invention includes a step of applying a resin composition to the surface of a first metal sheet to form a coating film, a step of laminating a second metal sheet on the coating film of the first metal sheet to form a metal laminate, and a step of crimping the metal laminate, the metal laminate may be produced using two metal sheets, or may be produced using three or more metal sheets. The multiple metal sheets may be metal sheets made of the same material and thickness, or may be metal sheets made of different materials and thicknesses. In this case, when a metal laminate plate is manufactured using three or more metal plates, the metal laminate plate may be manufactured by repeating a method including the steps of applying a resin composition to the surface of a first metal plate to form a coating film, laminating a second metal plate on the coating film of the first metal plate to form a metal laminate, pressing the metal laminate, applying a resin composition to the surface of the pressed metal laminate to form a coating film, further laminating a third metal plate on the coating film of the metal laminate to form a metal laminate, and pressing the metal laminate. Alternatively, the metal laminate plate may be manufactured by repeating a step of applying a resin composition to the surfaces of three or more metal plates to form coating films, and then laminating the metal plates to form a metal laminate multiple times, followed by pressing the metal laminate.

[0099] The method for producing a metal laminate plate of the present invention can obtain a strongly bonded metal laminate plate by producing it by the above-mentioned method using the above-mentioned resin composition. The metal laminate plate obtained by the present invention can be used without any particular limitation as long as it is used for applications in which metal laminate plates are used, for example, as a metal laminate plate for automobiles, vehicles (such as bullet trains and trains), civil engineering, architecture, ships, airplanes, and the space industry.

[0100] 4. Metal Laminate Plate The metal laminate plate of the present invention is a metal laminate plate formed by laminating a first metal plate, a coating film of the resin composition described above, and a second metal plate in this order. The first metal plate and the second metal plate may be metal plates made of the same material and thickness, or may be metal plates made of different materials and thicknesses. The metal laminate plate of the present invention can be manufactured, for example, by the above-described method for manufacturing a metal laminate plate. Since the metal plates of the metal laminate plate of the present invention are strongly bonded to each other, it can be used without particular limitation for any application in which a metal laminate plate is used. The metal laminate plate of the present invention can be used, for example, as a metal laminate plate for automobiles, vehicles (such as bullet trains and trains), civil engineering, construction, ships, airplanes, and the space industry.

[0101] The present disclosure includes the following aspects.

[0102] [1] A resin composition containing component (A) consisting of an epoxy resin that is solid at 25°C, and component (B) consisting of one or more members selected from the group consisting of polyether polyurethane prepolymers and polyether polyurethanes.

[0103] [2] The resin composition according to [1], wherein component (A) contains a bisphenol A-type epoxy resin that is solid at 25°C.

[0104] [3] The resin composition according to [1] or [2], wherein component (B) contains a polyether polyurethane prepolymer obtained by reacting a polyether polyol compound, a polyisocyanate compound, an anionic group-introducing agent, and a melamine-based compound.

[0105] [4] The resin composition according to any one of [1] to [3], wherein component (B) contains a polyether polyurethane obtained by reacting a polyether polyol compound, a polyisocyanate compound, an anionic group-introducing agent, and a melamine-based compound, followed by blocking with a blocking agent or chain extension with a chain extender.

[0106] [5] The resin composition according to any one of [1] to [4], wherein the ratio of the contents of component (A) and component (B) in the resin composition is 5:95 to 98:2 in mass ratio.

[0107] [6] The resin composition according to any one of [1] to [5], further containing water, wherein the water content is 10 to 90 mass%.

[0108] [7] A resin composition for metal surface treatment, comprising: component (A) consisting of an epoxy resin that is solid at 25°C; and component (B) consisting of one or more members selected from the group consisting of polyether polyurethane prepolymers and polyether polyurethanes.

[0109] [8] A method for producing a metal laminate plate, comprising: a step of applying the resin composition according to any one of [1] to [6] to the surface of a first metal plate to form a coating film; and a step of laminating a second metal plate onto the coating film of the first metal plate to form a metal laminate.

[0110] [9] The method for producing a metal laminate according to [8], further comprising a step of pressing the metal laminate.

[0111]

[10] A metal laminate plate obtained by laminating a first metal plate, a coating film of the resin composition according to any one of [1] to [6], and a second metal plate in this order.

[0112] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited thereto. In the following examples, percentages are by mass unless otherwise specified.

[0113] <Preparation of Epoxy Resin Water-Dispersed Emulsion 1> 290.0 g of bisphenol A epoxy resin (melting point 0°C or less, epoxy equivalent 190 g / eq.), 159.5 g of bisphenol A, and 0.1 g of triphenylphosphine as a catalyst were placed in a four-neck separable round-bottom flask equipped with a Dimroth stirrer, a stirring blade, and a nitrogen line, and the mixture was allowed to react at 180°C for 5 hours to obtain Epoxy Resin A-1. Subsequently, 50.5 g of propylene glycol monomethyl ether was added as a solvent, followed by the addition of 50.5 g of nonionic surfactant 1 having an ethylene oxide skeleton and a weight-average molecular weight of 16,000. The mixture was cooled to 70°C, and then 449.5 g of water was added to perform phase inversion emulsification, thereby producing Epoxy Resin Water-Dispersed Emulsion 1. The obtained water-dispersed epoxy resin emulsion 1 contained 45.0 mass% of epoxy resin A-1 (bisphenol A-type epoxy resin, melting point 140°C, epoxy equivalent 3,000 g / eq.), 5.0 mass% of nonionic surfactant 1, 5.0 mass% of propylene glycol monomethyl ether, and 45.0 mass% of water.

[0114] <Preparation of Epoxy Resin Water-Dispersed Emulsion 2> 450.5 g of bisphenol A-type epoxy resin (melting point 0°C or less, epoxy equivalent 190 g / eq.), 49.5 g of propylene glycol monomethyl ether as a solvent, and 49.5 g of nonionic surfactant 1 having an ethylene oxide skeleton and a weight-average molecular weight of 16,000 were added to a four-neck separable round-bottom flask equipped with a Dimroth stirrer, a stirring blade, and a nitrogen line, and the mixture was mixed at 70°C. 450.5 g of water was then added to effect phase inversion emulsification, thereby producing an epoxy resin water-dispersed emulsion 2. The resulting epoxy resin water-dispersed emulsion 2 contained 45.0 mass% of epoxy resin A'-2 (bisphenol A-type epoxy resin, melting point 0°C or less, epoxy equivalent 190 g / eq.), 5.0 mass% of nonionic surfactant 1, 5.0 mass% of propylene glycol monomethyl ether, and 45.0 mass% of water.

[0115] <Production of Urethane Resin Water-Dispersed Emulsion 1> Into a four-neck separable round-bottom flask equipped with a Dimroth stirrer, a stirring blade, and a nitrogen line, 202.7 g of polytetramethylene ether glycol having a number average molecular weight of 1,000 as a polyether polyol compound, 436.9 g of hydrogenated diphenylmethane diisocyanate as a polyisocyanate compound, 67.6 g of dimethylolpropionic acid as an anionic group introducing agent, 33.8 g of melamine, 56.3 g of triethylamine as a neutralizing agent, and 202.7 g of N-methyl-2-pyrrolidone were added, and the mixture was allowed to react at 80°C for 5 hours to produce a urethane prepolymer solution. Subsequently, 724.0 g of 40°C water was added to a 2L disposable cup and stirred, after which 500 g of the urethane prepolymer solution was added and stirred for 30 minutes. Thereafter, 52.0 g of an aqueous solution of ethylenediamine / water = 1 / 3 (mass ratio) was added, and the mixture was further stirred for 1 hour to obtain a water-dispersed urethane resin emulsion 1. The obtained water-dispersed urethane resin emulsion 1 contained 30 mass% of polyether polyurethane B-1 (acid value: 38.0 mg KOH / g, polyether structure content: 27 mass%), 8 mass% of N-methyl-2-pyrrolidone, and 62 mass% of water.

[0116] <Preparation of Urethane Resin Water-Dispersed Emulsion 2> A four-neck separable round-bottom flask equipped with a Dimroth stirrer, a stirring blade, and a nitrogen line was charged with 374.3 g of polytetramethylene ether glycol having a number average molecular weight of 1,000 as a polyether polyol compound, 334.2 g of hydrogenated diphenylmethane diisocyanate as a polyisocyanate compound, 42.8 g of dimethylolpropionic acid as an anionic group introducing agent, 13.4 g of melamine, 32.1 g of triethylamine as a neutralizing agent, and 203.2 g of N-methyl-2-pyrrolidone, and the resulting mixture was reacted at 80°C for 5 hours to produce a urethane prepolymer solution. Subsequently, 765.8 g of 40°C water was added to a 2 L disposable cup and stirred, after which 500 g of the urethane prepolymer solution was added and stirred for 30 minutes. Thereafter, 26.7 g of an aqueous solution of ethylenediamine / water = 1 / 3 (mass ratio) was added, and the mixture was further stirred for 1 hour to obtain a water-dispersed urethane resin emulsion 2. The obtained water-dispersed urethane resin emulsion 2 contained 30 mass% of polyether polyurethane B-2 (acid value: 23.0 mg KOH / g, polyether structure content: 49 mass%), 8 mass% of N-methyl-2-pyrrolidone, and 62 mass% of water.

[0117] <Production of Urethane Resin Water-Dispersed Emulsion 3> A four-neck separable round-bottom flask equipped with a Dimroth stirrer, a stirring blade, and a nitrogen line was charged with 253.2 g of polyester polyol having a number average molecular weight of 500, 436.7 g of hydrogenated diphenylmethane diisocyanate as a polyisocyanate compound, 50.6 g of dimethylolpropionic acid as an anionic group introducing agent, 19.0 g of melamine, 38.0 g of triethylamine as a neutralizing agent, and 202.5 g of N-methyl-2-pyrrolidone, and the resulting mixture was reacted at 80 ° C. for 5 hours to produce a urethane prepolymer solution. Subsequently, 771.1 g of water at 40 ° C. was added to a 2 L disposable cup and stirred. After stirring, 500 g of the urethane prepolymer solution was added and stirred for 30 minutes. Thereafter, 35.5 g of an aqueous solution of ethylenediamine / water = 1 / 3 (mass ratio) was added, and the mixture was further stirred for 1 hour to obtain a urethane resin water-dispersed emulsion 3. The resulting aqueous urethane resin emulsion 3 contained 30% by mass of polyester polyurethane B'-3 (acid value: 28.0 mgKOH / g), 8% by mass of N-methyl-2-pyrrolidone, and 62% by mass of water.

[0118] <Preparation of Urethane Resin Water-Dispersed Emulsion 4> A four-neck separable round-bottom flask equipped with a Dimroth stirrer, a stirring blade, and a nitrogen line was charged with 526.8 g of polycarbonate diol having a number average molecular weight of 2,000 as a polycarbonate polyol compound, 229.9 g of hydrogenated diphenylmethane diisocyanate as a polyisocyanate compound, 43.1 g of dimethylolpropionic acid as an anionic group introducing agent, 42.2 g of triethylamine as a neutralizing agent, and 202.2 g of N-methyl-2-pyrrolidone, and the reaction was carried out at 80°C for 5 hours to produce a urethane prepolymer solution. Subsequently, 807.8 g of 40°C water was added to a 2 L disposable cup and stirred, after which 500 g of the urethane prepolymer solution was added and stirred for 30 minutes. Thereafter, 22.3 g of an aqueous solution of ethylenediamine / water = 1 / 3 (mass ratio) was added, and the mixture was further stirred for 1 hour to obtain a water-dispersed urethane resin emulsion 4. The obtained water-dispersed urethane resin emulsion 4 contained 30 mass % of polycarbonate polyurethane B'-4 (acid value: 23.0 mgKOH / g), 8 mass % of N-methyl-2-pyrrolidone, and 62 mass % of water.

[0119] [Examples 1 to 4, Comparative Examples 1 to 5] The resin compositions of Examples 1 to 4 and Comparative Examples 1 to 5 shown in Table 1 were produced by mixing the produced water-dispersed epoxy resin emulsions 1 and 2 and the produced water-dispersed urethane resin emulsions 1 to 4.

[0120] [Room Temperature Adhesion Evaluation] The resin compositions produced in Examples 1 to 4 and Comparative Examples 1 to 5 were applied to one side of two steel plates (25 mm wide, 100 mm long, 1.6 mm thick) to a coating thickness of approximately 4 μm after drying, and then dried with hot air (at a sheet temperature of 200°C) to produce surface-treated steel plates with a coating film of the resin composition formed on the entire surface of each steel plate. The two surface-treated steel plates were stacked so that the treated surfaces (the surfaces on which the coating film was formed) of the surface-treated steel plates overlapped each other by 10 mm in the longitudinal direction (their positions in the width direction were the same), and the plates were pressed together at room temperature for 10 or 20 minutes under a pressure of 3 MPa using a press to produce a metal laminate plate with the two steel plates bonded together. The lap shear strength (MPa) of the resulting metal laminate plate was measured using a tensile tester according to the method described in JIS K 6850 (1999), and the adhesion was evaluated from the lap shear strength value according to the following room temperature adhesion evaluation criteria. The evaluation results of the room temperature adhesion of each resin composition are shown in Table 1. In this evaluation, if the room temperature adhesion rating is △ or higher, it indicates that the composition is practical for use in a short-term room temperature adhesion method.

[0121] Evaluation criteria for room temperature adhesiveness: ◎: Lap shear strength is 15 MPa or more; ○: Lap shear strength is 10 MPa or more but less than 15 MPa; △: Lap shear strength is 5 MPa or more but less than 10 MPa; ×: Lap shear strength is less than 5 MPa

[0122] [Evaluation of High-Temperature Adhesion] The resin compositions produced in Examples 1 to 4 and Comparative Examples 1 to 5 were applied to one side of two steel plates (25 mm wide, 100 mm long, 1.6 mm thick) to a coating thickness of approximately 4 μm after drying, and then dried with hot air (at a plate temperature of 200°C) to produce surface-treated steel plates with a coating film of the resin composition formed on the entire surface of each steel plate. The two surface-treated steel plates were stacked so that the treated surfaces (surfaces on which the coating film was formed) of the surface-treated steel plates overlapped by 10 mm in the longitudinal direction (their positions in the width direction were the same), and then pressure-bonded at 180°C for 10 minutes using a heater press while applying a pressure of 3 MPa to produce a metal laminate plate with two steel plates bonded together. The lap shear strength (MPa) of the obtained metal laminate plate was measured using a tensile tester according to the method described in JIS K 6850 (1999), and the adhesion was evaluated from the lap shear strength value according to the following evaluation criteria for high-temperature adhesion. The evaluation results of the high-temperature adhesiveness of each resin composition are shown in Table 1. In this evaluation, if the high-temperature adhesiveness rating is △ or higher, it indicates that the composition is practical for use in a high-temperature adhesive method for a short time.

[0123] Evaluation criteria for high temperature adhesiveness: ◎: Lap shear strength is 2.5 MPa or more; ○: Lap shear strength is 1.0 MPa or more and less than 2.5 Pa; △: Lap shear strength is 0.1 MPa or more and less than 1.0 MPa; ×: Lap shear strength is less than 0.1 MPa

[0124] [Corrosion Resistance Evaluation] The resin compositions produced in Examples 1 to 4 and Comparative Examples 1 to 5 were applied to one side of a steel plate (25 mm wide, 100 mm long, 1.6 mm thick) so that the coating thickness after drying was approximately 4 μm. The steel plate was then dried with hot air (reaching a plate temperature of 200°C) to produce surface-treated steel plates with a coating film of the resin composition formed on the entire surface of each steel plate. The surface-treated steel plates thus produced were subjected to a salt spray test at 35°C for 24 hours using 5% by mass of neutral salt water on the treated surface (the surface on which the coating film was formed) in accordance with JIS Z 2371 (2015). The corrosion resistance of each resin composition was evaluated by visual observation of the coating film on the surface-treated steel plate after the test and based on the corrosion resistance evaluation criteria described below. The corrosion resistance evaluation results for each resin composition are shown in Table 1. A corrosion resistance rating of Fair or higher in this evaluation indicates practical applicability.

[0125] Evaluation criteria for corrosion resistance: ◎: Rust occurred on less than 10% of the surface area. ○: Rust occurred on 10% or more but less than 20% of the surface area. △: Rust occurred on 20% or more but less than 40% of the surface area. ×: Rust occurred on 40% or more of the surface area.

[0126]

[0127] As shown in Table 1, the resin composition of the present invention, which contains component (A) consisting of an epoxy resin that is solid at 25°C and component (B) consisting of one or more components selected from the group consisting of polyether polyurethane prepolymers and polyether polyurethanes, exhibited excellent adhesive properties, particularly adhesive properties that allowed bonding by short-term compression bonding at room temperature and high temperatures, and corrosion resistance. On the other hand, when an epoxy resin that is liquid at 25°C was used instead of component (A), or when a polyester polyurethane or polycarbonate polyurethane was used instead of component (B), adhesive properties by short-term compression bonding were not obtained. These results demonstrate that the present invention can provide a resin composition with superior adhesive properties compared to conventional resin compositions.

Claims

1. A resin composition containing component (A) consisting of an epoxy resin that is solid at 25°C and component (B) consisting of one or more components selected from the group consisting of polyether polyurethane prepolymers and polyether polyurethanes.

2. The resin composition according to claim 1, wherein the component (A) contains a bisphenol A type epoxy resin that is solid at 25°C.

3. The resin composition according to claim 1, wherein the component (B) contains a polyether polyurethane prepolymer obtained by reacting a polyether polyol compound, a polyisocyanate compound, an anionic group introducing agent, and a melamine compound.

4. The resin composition according to claim 1, wherein the component (B) contains a polyether polyurethane obtained by reacting a polyether polyol compound, a polyisocyanate compound, an anionic group introducing agent, and a melamine compound, followed by blocking with a blocking agent or chain extension with a chain extender.

5. The resin composition according to claim 1, wherein the ratio of the contents of said component (A) and said component (B) in said resin composition is 5:95 to 98:2 in terms of mass ratio.

6. The resin composition according to claim 1, further comprising water, the water content being 10 to 90 mass %.

7. A resin composition for metal surface treatment, comprising component (A) an epoxy resin that is solid at 25°C and component (B) consisting of one or more components selected from the group consisting of polyether polyurethane prepolymers and polyether polyurethanes.

8. A method for producing a metal laminate plate, comprising the steps of: applying the resin composition according to any one of claims 1 to 6 to the surface of a first metal plate to form a coating film; and laminating a second metal plate onto the coating film of the first metal plate to form a metal laminate.

9. The method of claim 8, further comprising the step of crimping the metal laminate.

10. A metal laminate plate comprising a first metal plate, a coating film of the resin composition according to any one of claims 1 to 6, and a second metal plate laminated in this order.

Citation Information

Patent Citations

  • Aqueous composition used in production of crosslinked polyurethane

    JP1990003465A

  • Improved aqueous emulsion based on polyol and hindered isocyanate compound

    JP1992359081A

  • Aqueous polyurethane dispersion

    JP1993230364A

  • Water-base baking coating composition for metallic can

    JP1995053916A

  • Production of aqueous polyurethane composition having discoloration resistance

    JP1996113704A