Copolymer and contact lens treatment solution
Patent Information
- Application Number
- PCT/JP2024/010658
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-19
- Publication Date
- 2024-10-03
AI Technical Summary
Existing contact lens treatment methods fail to maintain hydrophilicity and lubricity on soft contact lenses for an extended period, leading to temporary comfort and economic disadvantages due to complex and costly manufacturing processes.
A novel copolymer is developed by copolymerizing specific monomers with structural units represented by formulas (A) and (B), with a molar ratio of 10-80 mol% and 20-90 mol% respectively, and a weight average molecular weight of 10,000 to 2,000,000, which is incorporated into a contact lens treatment liquid to impart long-lasting hydrophilicity and lubricity.
The copolymer effectively maintains excellent hydrophilicity and lubricity on soft contact lenses, enhancing wearing comfort throughout the day and reducing manufacturing costs by simplifying the treatment process.
Smart Images

Figure JP2024010658_03102024_PF_FP_ABST
Abstract
Description
Copolymer and treatment solution for contact lenses
[0001] The present invention relates to a copolymer and a contact lens treatment solution.
[0002] Conventionally, surface treatment agents have been widely proposed that can impart surface hydrophilicity, biocompatibility, antithrombogenicity, etc. due to phosphorylcholine groups by treating the surfaces of various materials with phosphorylcholine group-containing copolymers. Applications include hydrophilization treatments for hydrophobic substrates, antifouling treatments for industrial filter surfaces, and surface treatments for suppressing protein and cell adsorption on medical polymer materials. In particular, in recent years, they have been used for soft contact lenses.
[0003] The wearing comfort of soft contact lenses is largely dependent on the hydrophilicity and lubricity of the lens surface, and maintaining these properties over a long period of time leads to sustained, comfortable wearing all day.
[0004] As techniques for maintaining the wearing comfort of lenses, for example, the techniques described in Patent Documents 1 and 2 are known. Patent Document 1 discloses a technique in which a soft contact lens is subjected to a plasma treatment and subjected to a hydrophilization treatment with a zwitterionic group. Furthermore, Patent Document 2 discloses a technique in which a soft contact lens containing a reactive group is chemically reacted with a hydrophilic polymer having a reactive group to bond the soft contact lens surface, thereby hydrophilizing the soft contact lens surface. These techniques impart hydrophilicity to the surface by treating the soft contact lens itself, and because the treatment process is complicated, highly controlled manufacturing facilities tailored to the treatment technology are required, which is economically disadvantageous.
[0005] As a technique for solving such problems, for example, Patent Documents 3, 4, and 5 disclose a technique in which polyethylene glycol or a cellulose-based polymer is blended into a treatment solution for soft contact lenses to impart and enhance hydrophilicity to the surface of the soft contact lens, thereby improving the wearing comfort.
[0006] Furthermore, phosphorylcholine group-containing polymers have a structure similar to phospholipids derived from biological membranes and are known to have excellent properties such as very high hydrophilicity and high moisturizing properties. For example, Patent Document 6 discloses a technology in which a copolymer of a phosphorylcholine group-containing monomer and butyl methacrylate is added to a treatment solution for soft contact lenses to improve wearing comfort.
[0007] International Publication No. WO 2010 / 092686, International Publication No. WO 2001 / 074932, International Publication No. WO 2009 / 032122, International Publication No. WO 2012 / 098653, International Publication No. WO 2008 / 060798, U.S. Patent Application Publication No. 2009 / 0100801
[0008] However, although the contact lenses using the soft contact lens treatment solutions described in Patent Documents 3, 4, 5 and 6 provide excellent wearing comfort in the early stages of wearing, the copolymer and the blended components are not sufficiently adsorbed onto the contact lens surface, and the good wearing comfort is only sustained temporarily.
[0009] In view of the above problems, an object of the present invention is to provide a copolymer that can easily impart hydrophilicity and lubricity to the surface of a soft contact lens and maintain these properties for a long period of time, and a contact lens treatment solution using the copolymer.
[0010] As a result of extensive research, the present inventors have found that the above-mentioned object can be achieved by a novel copolymer obtained by copolymerizing at least two specific types of monomers, and have thus completed the present invention.
[0011] That is, the present invention comprises the following [1] to [4]. [1]. A copolymer having constitutional units represented by the following formulas (A) and (B), wherein the molar ratio n of the constitutional unit represented by the following formula (A) to the entire copolymer is: A is 10 to 80 mol %, and the molar ratio n of the structural unit represented by the following formula (B) to the entire copolymer is B and a weight average molecular weight of 10,000 to 2,000,000. [In the formula (A) and formula (B), R 1 and R 2Each of X in formula (A) independently represents a hydrogen atom or a methyl group. 3 , where R 3 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 4 O represents an oxyalkylene group having 2 to 4 carbon atoms, and R 4 O contains at least two types of oxyalkylene groups with different carbon numbers, and the addition form thereof may be either block or random, and p represents the average number of moles of oxyalkylene groups added, which is a number from 4 to 100.] [2]. The copolymer has a structural unit represented by the following formula (C) or (D), and the molar ratio n of the structural unit represented by the following formula (C) or (D) to the entire copolymer: C and n D The copolymer according to [1], wherein the total of is more than 0 mol% and 50 mol% or less. [In the formula (C), R 5 is H or a methylene group, and R 6 is an alkyl group having 1 to 5 carbon atoms, or R 5 is a methylene group, the terminal is R 5 In formula (D), R is an alkylene group having 1 to 5 carbon atoms that is bonded to the 7 is a hydrogen atom or a methyl group, and Y is O or NR 10 , where R 10 is H or an alkyl group having 1 to 4 carbon atoms, and when Y is O, E 1 is a structure represented by formula (E), and Y is NR 10 In the case of E 1 is a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or a structure represented by formula (E). 8 is H or an alkyl group having 1 to 4 carbon atoms, R 9is a hydrogen atom or an alkyl group having 1 to 18 carbon atoms.] [3]. The copolymer according to [1] or [2], wherein the structural unit (A) is a structural unit derived from 2-(methacryloyloxy)ethyl 2-(trimethylammonio)ethyl phosphate. [4]. A contact lens treatment solution containing 0.001 w / v % or more and 5.0 w / v % or less of the copolymer (P) according to any one of [1] to [3].
[0012] The copolymer of the present invention can impart excellent hydrophilicity and lubricity, and these properties are sustained, to the surface of a soft contact lens, and therefore the copolymer of the present invention is suitable as a treatment solution for a soft contact lens.
[0013] Figure 1 shows the w in the chromatogram (vertical axis: refractive index intensity, horizontal axis: retention time). b and w f 1 is a diagram for explaining the above.
[0014] The present invention will be described in detail below.
[0015] In this specification, "(meth)acrylate" means "acrylate or methacrylate," and the same applies to other similar terms. Furthermore, in this specification, the alkyl group may be linear or branched.
[0016] In this specification, "all day" refers to the period from the start of wearing contact lenses to the end of wearing them, and is intended to be 8 to 16 hours of continuous wear. "Long-term" refers to the entire day of wearing contact lenses.
[0017] Furthermore, in this specification, when preferred numerical ranges (e.g., ranges of concentration or weight-average molecular weight) are described in stages, the respective lower and upper limits can be independently combined. For example, in the description "preferably 10 or more, more preferably 20 or more, and preferably 100 or less, more preferably 90 or less," the "preferable lower limit: 10" and the "more preferable upper limit: 90" can be combined to form "10 or more and 90 or less." Furthermore, in the description "preferably 10 to 100, more preferably 20 to 90," the range can be similarly set to "10 to 90."
[0018] The product forms of the composition containing the copolymer of the present invention include compositions to be applied directly to the eye and compositions used to treat devices worn on the eye, such as contact lenses, and can be specified as follows. Specific examples include contact lens treatment solutions. Specific product forms of the contact lens treatment solution of the present invention include contact lens packing solutions (contact lens shipping solutions), contact lens storage solutions, contact lens cleaning solutions, contact lens cleaning and storage solutions, contact lens disinfectants, contact lens wear aids, etc.
[0019] In this specification, the shipping solution for soft contact lenses refers to a solution that is sealed in a packaging container such as a blister package together with soft contact lenses when the soft contact lenses are distributed. Generally, soft contact lenses are used in a state swollen with an aqueous solution, and therefore the lenses are sealed in a packaging container in a state swollen with an aqueous solution at the time of shipment from the factory so that they can be used immediately.
[0020] <Copolymer (P)> The copolymer (P) of the present invention contains constitutional units represented by the following formulas (A) and (B), and the molar ratio n of the constitutional unit represented by the following formula (A) to the entire copolymer (P) is A is 10 to 80 mol %, and the molar ratio n of the structural unit represented by the following formula (B) to the entire copolymer (P) is B is 20 to 90 mol % and the weight average molecular weight is 10,000 to 2,000,000.
[0021]
[0022] In the formula (A) and formula (B), R 1 and R 2 Each of X in formula (A) independently represents a hydrogen atom or a methyl group. 3 , where R 3 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 4 O represents an oxyalkylene group having 2 to 4 carbon atoms, and R 4O contains at least two kinds of oxyalkylene groups having different carbon numbers, and the addition form thereof may be either block or random. p represents the average number of moles of oxyalkylene groups added and is a number of 4 to 100.
[0023] [Structural Unit Represented by Formula (A)] The copolymer (P) used in the present invention has a structural unit represented by general formula (A). This structural unit is obtained by polymerizing a monomer having a phosphorylcholine structure represented by the following general formula (a) (hereinafter also referred to as a "PC monomer"). By including a structural unit derived from a PC monomer in the copolymer (P), hydrophilicity can be imparted to the soft contact lens.
[0024]
[0025] In the formula (A) and formula (a), R 1 represents a hydrogen atom or a methyl group, and X represents O or NR 3 , where R 3 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
[0026] The PC monomer is preferably 2-((meth)acryloyloxy)ethyl 2-(trimethylammonio)ethyl phosphate, and more preferably 2-(methacryloyloxy)ethyl 2-(trimethylammonio)ethyl phosphate (hereinafter also referred to as "2-methacryloyloxyethyl phosphorylcholine") represented by the following formula (a'):
[0027]
[0028] The content of the structural unit represented by formula (A) in the copolymer (P) (molar ratio n A The molar ratio n is 10 to 80 mol %, preferably 15 to 75 mol %, more preferably 25 to 65 mol %, and even more preferably 30 to 55 mol %. A If the molar ratio n is less than 10 mol %, the effect of improving the hydrophilicity of the soft contact lens surface cannot be expected. AIf the molar ratio n is more than 80 mol %, the content of the structural unit represented by formula (B) will be small, the adsorption force of the copolymer (P) to the surface of the soft contact lens will be reduced, and the durability of the good wearing comfort will be insufficient. A When the ratio of the structural unit represented by formula (A) to the structural unit represented by formula (B) is 80 mol % or less, the effect of improving the hydrophilicity and lubricity of the soft contact lens surface can be further enhanced by adjusting the ratio of the structural unit represented by formula (A) to the structural unit represented by formula (B).
[0029] [Structural Unit Represented by Formula (B)] The copolymer (P) used in the present invention has a structural unit represented by the following formula (B). This structural unit is obtained by polymerizing a monomer represented by the following general formula (b), i.e., a monomer having a polyalkylene glycol structure (hereinafter also referred to as a "PAG monomer"). When the copolymer (P) contains a structural unit derived from a PAG monomer, the obtained soft contact lens maintains a good wearing comfort when worn. Furthermore, by having a structural unit represented by formula (A) and a structural unit represented by formula (B), the effect of improving the hydrophilicity and lubricity of the soft contact lens surface is further enhanced.
[0030] The copolymer (P) may also contain a plurality of structural units represented by the following (B) having different values of p.
[0031]
[0032] In the formulas (B) and (b), R 2 represents a hydrogen atom or a methyl group. 4 O represents an oxyalkylene group having 2 to 4 carbon atoms, and R 4 O contains at least two kinds of oxyalkylene groups with different carbon numbers. For example, the formula (b) contains an oxyethylene group (—CH 2 CH 2 O-), oxypropylene group (-CH(CH 3 ) CH 2 O-, -CH 2 CH (CH 3 )O—), oxybutylene group (—CH(CH 2 CH 3 ) CH 2O-, -CH 2 CH (CH 2 CH 3 )O-,-CH(CH 3 ) CH(CH 3 )O-), and R 4 The addition form of O may be either block or random, and p represents the average number of moles of oxyalkylene groups added, and is a number from 4 to 100.
[0033] The oxyalkylene group in formulas (B) and (b) preferably has a form consisting of an oxyethylene group and an oxypropylene group, an oxyethylene group and an oxybutylene group, an oxypropylene group and an oxybutylene group, or an oxypropylene group, an oxyethylene group and an oxybutylene group, and more preferably has a form consisting of an oxyethylene group and an oxypropylene group.
[0034] Furthermore, with regard to the number of moles of oxyethylene groups, oxypropylene groups, and oxybutylene groups added, the molar ratio of oxyethylene groups to the number of moles of all oxyalkylene groups added is 0 to 90%, preferably 40 to 90%, and more preferably 60 to 80%. The molar ratio of oxypropylene groups added is 0 to 70%, more preferably 10 to 50%, and the molar ratio of oxybutylene groups added is 0 to 70%, more preferably 0 to 30%. When the molar ratio of oxyethylene groups added is greater than 90%, the proportions of oxypropylene groups and oxybutylene groups decrease relatively, resulting in a decrease in the adsorptivity to the contact lens surface. On the other hand, when the proportion of oxypropylene groups and oxybutylene groups exceeds 70%, the cohesive strength between the copolymers (P) becomes excessive, resulting in a decrease in the transparency of the resulting contact lens treatment solution and the contact lens after treatment.
[0035] The monomer represented by formula (b) is calculated from a chromatogram (vertical axis: refractive index intensity, horizontal axis: retention time) obtained by gel permeation chromatography (GPC) measurement using a differential refractometer. b And lol f The ratio of b / w f However, the formula (1) is: 1.10≦wb / w f ≦2.50 (1) (In formula (1), the retention time at the maximum peak height (h) in the peak of the chromatogram is t h and 1 / 10 of the maximum peak height (h 1/10 ) are two retention times at t f and t b (However, t f <t b ) and then w f is h and f The difference between (t h -t f ), and w b is b and h The difference between (t b -t h ) is preferably satisfied (see FIG. 1).
[0036] W of monomer (b) b / w f When w is smaller than 1.10, the molecular weight distribution of the monomer (b) is biased more to the high molecular weight side, the concentration of the polymerizable functional group is lowered, and the polymerizability of the monomer (b) may be reduced. b / w f is preferably 1.20 or more, and more preferably 1.30 or more.
[0037] On the other hand, the w of monomer (b) b / w f If w is greater than 2.50, the adsorption force of the copolymer (P) to the surface of a soft contact lens may decrease. b / w f is 2.00 or less, more preferably 1.80 or less.
[0038] w b / w fThe chromatogram (vertical axis: refractive index intensity, horizontal axis: retention time) for calculating the above was obtained using an HLC-8320GPC (registered trademark) gel permeation chromatography (GPC) system, a SHODEXKF-G guard column, and three SHODEXKF804L columns connected in series, with the column temperature set to 40°C and tetrahydrofuran as a developing solvent flowing at a flow rate of 1 mL / min, and 0.1 mL of a 0.1 wt % tetrahydrofuran solution of polyalkylene glycol mono(meth)acrylate injected, using an EcoSEC GPC calculation program.
[0039] The content of the structural unit represented by formula (B) in the copolymer (P) (molar ratio n B ) is 20 to 90 mol %, preferably 25 to 85 mol %, more preferably 35 to 75 mol %, and even more preferably 45 to 70 mol %. As described above, the copolymer (P) used in the present invention has the monomer represented by formula (B) as a constituent unit, and therefore the adsorptive power of the copolymer (P) to the surface of a soft contact lens can be improved, resulting in good wearing comfort.
[0040] The content of the structural unit represented by formula (B) (molar ratio n B ) is the content (molar ratio n A This further enhances the effect of improving the hydrophilicity and lubricity of the soft contact lens surface. A and molar ratio n B The ratio of (n B / n A ) is preferably 0.5 to 7.0, more preferably 1.0 to 3.0.
[0041] In the formula (B), p is 4 to 100, preferably 5 to 70, and more preferably 7 to 40. If p is less than 4, the adsorptive force of the copolymer (P) to the surface of a soft contact lens decreases, and if it is greater than 100, the cohesive force between the copolymers (P) increases, resulting in a deterioration in the transparency of the resulting contact lens treatment solution and the contact lens after treatment.
[0042] The compound represented by formula (b) can be produced by adding ethylene oxide, propylene oxide, or butylene oxide (preferably propylene oxide or ethylene oxide) to a starting material (e.g., 2-hydroxypropyl methacrylate) in the presence of a composite metal cyanide complex catalyst (hereinafter sometimes referred to as a "DMC catalyst"). Specifically, the starting materials and the DMC catalyst are placed in a reaction vessel, and, under stirring in an inert gas atmosphere, at least two of ethylene oxide, propylene oxide, or butylene oxide (hereinafter collectively referred to as "alkylene oxides having 2 to 4 carbon atoms") are added continuously or intermittently to carry out addition polymerization. The alkylene oxides having 2 to 4 carbon atoms may be added under pressure or at atmospheric pressure.
[0043] The reaction temperature for adding an alkylene oxide having 2 to 4 carbon atoms to a starting material is preferably 50° C. to 120° C., more preferably 70° C. to 90° C. If the reaction temperature is lower than 50° C., the reaction rate is very slow, and if it is higher than 120° C., problems such as polymerization of polymerizable groups in the starting material and coloration occur.
[0044] As the DMC catalyst in the present invention, known ones can be used, for example, the DMC catalyst described in JP-A-2022-130139 can be used.
[0045] A particularly preferred DMC catalyst is Zn(II) 3 [Co(III)(CN) 6 ] 2 (H 2 O) 4 (tert-butyl alcohol) 2 is.
[0046] The amount of the DMC catalyst used is not particularly limited, but is preferably 0.0001 to 0.1 parts by mass, more preferably 0.001 to 0.05 parts by mass, per 100 parts by mass of the monomer represented by formula (b). The DMC catalyst may be added to the reaction system all at once at the beginning, or may be added in portions one by one. After the polymerization reaction is completed, the DMC catalyst is removed. The catalyst can be removed by known methods such as filtration, centrifugation, or treatment with a synthetic adsorbent.
[0047] Other additives may be used in the reaction of adding an alkylene oxide having 2 to 4 carbon atoms to a starting material. For example, polymerization inhibitors such as hydroquinone (HQ), hydroquinone monomethyl ether (MQ), 2,6-di-tert-butylhydroxytoluene (BHT), di-tert-butylhydroxyanisole (BHA), α-tocopherol, β-tocopherol, and γ-tocopherol can be added to the reaction system. The polymerization inhibitor is preferably MQ and / or BHT, more preferably BHT. The amount of polymerization inhibitor added is preferably 0.001 to 0.3 parts by mass per 100 parts by mass of the total of the starting material (e.g., 2-hydroxypropyl methacrylate) and the alkylene oxide having 2 to 4 carbon atoms. If this amount is less than 0.001 part by mass, the polymerization inhibitor may function insufficiently, potentially causing gelation during the addition of the alkylene oxide having 2 to 4 carbon atoms. If the amount added is more than 0.3 parts by mass, the purity of the compound of formula (1b') obtained may be low.
[0048] [Structural units represented by formulas (C) and (D)] The copolymer (P) used in the present invention can contain a structural unit represented by the following formula (C) or (D). The structural unit is obtained by polymerizing a monomer represented by the following general formula (c) or (d), respectively. When the copolymer (P) contains (c) or (d), the adhesive force of the copolymer (P) to soft contact lenses is more likely to be maintained, depending on the type of contact lens, and a good wearing comfort can be maintained.
[0049]
[0050]
[0051] In the formulas (C) and (c), R 5 is H or a methylene group, and R 6 is an alkyl group having 1 to 5 carbon atoms, or R 5 is a methylene group, R 5 In formulas (D) and (d), R is an alkylene group having 1 to 5 carbon atoms that is bonded to the 7is a hydrogen atom or a methyl group, and Y is O or NR 10 , where R 10 is H or an alkyl group having 1 to 4 carbon atoms, and when Y is O, E 1 is a structure represented by formula (E), and Y is NR 10 In the case of E 1 is a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or a structure represented by formula (E). 8 is H or an alkyl group having 1 to 4 carbon atoms, R 9 represents a hydrogen atom or an alkyl group having 1 to 18 carbon atoms.
[0052] Examples of the monomer represented by formula (c) include N-vinylpyrrolidone, N-vinylcaprolactam, N-vinylformamide, N-vinylacetamide, N-methyl-N-vinylacetamide, etc. Examples of the monomer represented by formula (d) include N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-propyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-butyl(meth)acrylamide, N-tert-butyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, 2-(acetylamino)ethyl(meth)acrylate, 2-(stearamido)ethyl(meth)acrylate, 2-palmitamidoethyl(meth)acrylate, etc.
[0053] When the copolymer (P) contains the structural units represented by formula (C) and (D), the content of the structural unit represented by formula (C) in the copolymer (P) (molar ratio n C ) and the content of the structural unit represented by formula (D) (molar ratio n D The total of these is preferably more than 0 mol % and not more than 50 mol %, more preferably 10 to 50 mol %.
[0054] E in the formula (d) 1 The monomer represented by formula (E) can be synthesized, for example, by an esterification reaction between an alcohol having an amide structure at its terminal and (meth)acrylic acid or (meth)acrylic acid chloride, as described in JP-A-2017-160380.
[0055] [Other Monomers] The copolymer (P) may contain other polymerizable monomers other than the PC monomer, PAG monomer, and the structural units represented by (c) or (d), provided that the effects of the present invention are not impaired. The blending ratios thereof can be appropriately selected within a range that does not affect the effects of the present invention, but it is preferred that the copolymer (P) consists of only the PC monomer and PAG monomer.
[0056] Examples of the other monomer include polymerizable monomers selected from linear or branched alkyl (meth)acrylates, cyclic alkyl (meth)acrylates, aromatic group-containing (meth)acrylates, styrene-based monomers, vinyl ether monomers, vinyl ester monomers, hydroxyl group-containing (meth)acrylates, carboxy group-containing monomers, and sulfonyl group-containing monomers.
[0057] Examples of linear or branched alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, and triethylene glycol di(meth)acrylate. Examples of cyclic alkyl (meth)acrylates include cyclohexyl (meth)acrylate. Examples of aromatic group-containing (meth)acrylates include benzyl (meth)acrylate and phenoxyethyl (meth)acrylate. Examples of styrene-based monomers include styrene, methylstyrene, and chlorostyrene. Examples of vinyl ether monomers include methyl vinyl ether, propyl vinyl ether, butyl vinyl ether, triethylene glycol divinyl ether, and ethylene glycol monovinyl ether. Examples of vinyl ester monomers include vinyl acetate and vinyl propionate. Examples of hydrophilic hydroxyl group-containing (meth)acrylates include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and glycerol (meth)acrylate. Examples of carboxyl group-containing monomers and sulfonyl group-containing monomers include (meth)acrylic acid, styrenesulfonic acid, and (meth)acryloyloxyphosphonic acid.
[0058] [Weight-average molecular weight of copolymer (P)] The weight-average molecular weight of copolymer (P) is 10,000 to 2,000,000, preferably 20,000 or more, more preferably 30,000 or more, even more preferably 40,000 or more, and preferably 1,000,000 or less, more preferably 500,000 or less, and even more preferably 300,000 or less.
[0059] If the weight-average molecular weight is less than 10,000, the adsorption force to the soft contact lens surface will be reduced, and the effect of the copolymer (P) on the soft contact lens surface may not be maintained.If the weight-average molecular weight is more than 2,000,000, the viscosity may increase, making handling difficult.
[0060] The weight average molecular weight of the copolymer (P) refers to a value measured by gel permeation chromatography (GPC).
[0061] [Method for producing copolymer (P)] The copolymer (P) can be prepared by copolymerizing the above-mentioned monomers, and is usually a random copolymer. However, it may be an alternating copolymer or a block copolymer in which the individual monomers are regularly arranged, or may have a graft structure in part.
[0062] Specifically, for example, the copolymer (P) can be obtained by radical polymerization of a mixture of the monomers in the presence of a radical polymerization initiator under an inert gas atmosphere such as nitrogen, carbon dioxide, argon, or helium.
[0063] The radical polymerization method can be carried out by a known method such as bulk polymerization, suspension polymerization, emulsion polymerization, solution polymerization, etc. Of the radical polymerization methods, solution polymerization is preferred from the viewpoint of purification, etc. The copolymer (P) can be purified by a general purification method such as reprecipitation, dialysis, ultrafiltration, etc.
[0064] Examples of the radical polymerization initiator include an azo radical polymerization initiator, an organic peroxide, and a persulfate. Examples of the azo radical polymerization initiator include 2,2'-azobis(2-methylpropionamidine) dihydrochloride (V-50), 2,2'-azobis(2-diaminopropyl) dihydrochloride, 2,2'-azobis(2-(5-methyl-2-imidazolin-2-yl)propane) dihydrochloride, 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobisisobutylamide dihydrate, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobisisobutyronitrile (AIBN). Examples of organic peroxides include t-butyl peroxyneodecanate (Perbutyl (registered trademark) ND), benzoyl peroxide, diisopropyl peroxydicarbonate, t-butylperoxy-2-ethylhexanoate, t-butyl peroxypivalate, t-butylperoxyisobutyrate, lauroyl peroxide, t-butyl peroxydecanoate, and succinic acid peroxide (succinyl peroxide). Examples of persulfates include ammonium persulfate, potassium persulfate, and sodium persulfate. These radical polymerization initiators can be used alone or in combination of two or more. The amount of polymerization initiator used is usually 0.001 to 10 parts by mass, preferably 0.02 to 5.0 parts by mass, and more preferably 0.03 to 3.0 parts by mass, per 100 parts by mass of the total of the monomers.
[0065] The polymerization reaction of the copolymer (P) can be carried out in the presence of a solvent. The solvent is not particularly limited as long as it dissolves each monomer composition and is not reactive with the solvent itself. Examples of the solvent include water, alcohol solvents, ketone solvents, ester solvents, linear or cyclic ether solvents, and nitrogen-containing solvents. Examples of alcohol solvents include methanol, ethanol, n-propanol, and isopropanol. Examples of ketone solvents include acetone, methyl ethyl ketone, and diethyl ketone. Examples of ester solvents include ethyl acetate. Examples of linear or cyclic ether solvents include ethyl cellosolve and tetrahydrofuran. Examples of nitrogen-containing solvents include acetonitrile, nitromethane, and N-methylpyrrolidone. Among these solvents, a mixed solvent of water and alcohol is preferred.
[0066] [Concentration of Copolymer (P)] The concentration of copolymer (P) in the soft contact lens treatment solution of the present invention is 0.001 w / v% or more, preferably 0.01 w / v% or more, more preferably 0.05 w / v% or more, and 5.0 w / v% or less, preferably 2.0 w / v% or less, more preferably 1.0 w / v% or less. If the concentration of copolymer (P) is less than 0.001 w / v%, the amount of copolymer (P) added is so small that sufficient hydrophilicity and lubricity, and their durability, cannot be imparted. If the concentration exceeds 5.0 w / v%, sterile filtration during production may become difficult.
[0067] In the present invention, "w / v %" refers to the mass of a component in 100 mL of solution, expressed in grams (g). For example, "the treatment solution of the present invention contains 1.0 w / v % of copolymer (P)" means that 100 mL of the solution contains 1.0 g of copolymer (P).
[0068] The solvent used in the treatment liquid of the present invention may be water, alcohols such as ethanol, n-propanol, isopropanol, glycerol, or propylene glycol, or a mixture thereof. Water or a mixture of water and an alcohol is preferred, and water is more preferred.
[0069] The water used in the contact lens treatment solution of the present invention can be water typically used in the production of pharmaceuticals and medical devices, such as ion-exchanged water, purified water, sterilized purified water, distilled water, and water for injection.
[0070] [Other Components] In addition to the polymer (P), the contact lens treatment solution of the present invention may contain other components, such as vitamins, amino acids, sugars, thickeners, cooling agents, inorganic salts, organic acid salts, acids, bases, antioxidants, stabilizers, and preservatives, as needed. Examples of vitamins include flavin adenine dinucleotide sodium, cyanocobalamin, retinol acetate, retinol palmitate, pyridoxine hydrochloride, panthenol, sodium pantothenate, and calcium pantothenate. Examples of amino acids include aspartic acid or its salts, and aminoethylsulfonic acid. Examples of sugars include glucose, mannitol, sorbitol, xylitol, and trehalose. Examples of thickeners include hydroxypropylmethylcellulose and hydroxyethylcellulose. Examples of cooling agents include menthol and camphor. Examples of inorganic salts include sodium chloride, potassium chloride, disodium hydrogen phosphate, sodium dihydrogen phosphate, anhydrous sodium dihydrogen phosphate, potassium dihydrogen phosphate, and dipotassium hydrogen phosphate. Examples of salts of organic acids include sodium citrate. Examples of acids include phosphoric acid, citric acid, sulfuric acid, acetic acid, hydrochloric acid, and boric acid. Examples of bases include potassium hydroxide, sodium hydroxide, borax, trishydroxymethylaminomethane, and monoethanolamine. Examples of antioxidants include tocopherol acetate and dibutylhydroxytoluene. Examples of stabilizers include sodium edetate, glycine, and taurine. Examples of preservatives include benzalkonium chloride, chlorhexidine gluconate, potassium sorbate, methylparaben, ethylparaben, propylparaben, isopropylparaben, butylparaben, isobutylparaben, polyhexanide hydrochloride, and sulfamexazole.
[0071] [pH of Contact Lens Treatment Solution] From the viewpoint of improving wearing comfort, the pH of the contact lens treatment solution of the present invention is preferably 3.0 to 8.0, more preferably 3.5 to 7.8, even more preferably 4.0 to 7.6, and even more preferably 4.5 to 7.5. The pH of the contact lens treatment solution in this specification refers to the value measured in accordance with the 18th Edition of the Japanese Pharmacopoeia, General Test Method, 2.54, pH Measurement Method.
[0072] [Osmotic Pressure and Osmotic Pressure Ratio of Contact Lens Treatment Solution] From the viewpoint of improving wearing comfort, the osmotic pressure of the contact lens treatment solution of the present invention is preferably 200 to 400 mOsm, more preferably 225 to 375 mOsm, even more preferably 230 to 350 mOsm, and even more preferably 240 to 340 mOsm. The osmotic pressure ratio is preferably 0.7 to 1.4, more preferably 0.7 to 1.3, and even more preferably 0.8 to 1.2. Note that the osmotic pressure of the contact lens treatment solution in this specification refers to the value measured in accordance with the 18th Edition Japanese Pharmacopoeia, General Test Method 2.47, Osmolality Measurement Method (Osmolality Measurement Method), and the osmotic pressure ratio refers to the value obtained by dividing the obtained osmotic pressure value by the osmotic pressure value of 0.9% by mass physiological saline (286 mOsm).
[0073] [Method for producing soft contact lens treatment solution] The soft contact lens treatment solution of the present invention can be produced by a general method for producing a contact lens solution. For example, it can be produced by mixing and stirring the polymer (P), a solvent and other components as needed. The obtained soft contact lens treatment solution may be subjected to a procedure such as sterile filtration as needed.
[0074] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. The copolymers used in the examples and comparative examples are as follows.
[0075] Synthesis of Compound I Represented by Formula (b) [Synthesis Example 1-1] A 5 L autoclave equipped with a thermometer, pressure gauge, safety valve, nitrogen gas inlet tube, stirrer, vacuum exhaust tube, cooling coil, and steam jacket was charged with 500 g of 2-hydroxypropyl methacrylate (HPMA), 0.07 g of DMC catalyst, and 1.0 g of 2,6-di-tert-butylhydroxytoluene (BHT). After nitrogen substitution, the temperature was raised to 80°C, and 403 g of propylene oxide (PO) was added dropwise from the nitrogen gas inlet tube at 0.3 MPa or less. The changes in pressure and temperature in the reaction vessel over time were measured, and after 5 hours, the pressure in the reaction vessel suddenly decreased. Thereafter, while maintaining the reaction vessel at 80°C, a mixture of 262 g of PO and 870 g of ethylene oxide (EO) was gradually added dropwise from the nitrogen gas inlet tube at 0.5 MPa or less. After the addition was completed, the reaction was carried out at 80°C for 1 hour, and the reaction mixture was extracted from the reaction layer and filtered to remove solids, thereby obtaining a liquid product of the monomer of formula (b) in which 2 moles of PO were added to HPMA, and then 1.3 moles of PO and 5.7 moles of EO were added randomly. When the molecular weight distribution was confirmed by GPC, it was found that w b / w f The structure was 1 The DMC catalyst used was synthesized according to the procedure described in JP-A-2022-130139.
[0076] <Synthesis of Compound II Represented by Formula (b)> [Synthesis Example 1-2] A 5L autoclave equipped with a thermometer, pressure gauge, safety valve, nitrogen gas inlet tube, stirrer, vacuum exhaust tube, cooling coil, and steam jacket was charged with 520g of HPMA, 0.08g of DMC catalyst, and 1.0g of BHT. After nitrogen substitution, the temperature was raised to 80 ° C., and under conditions of 0.3 MPa or less, PO419g was added dropwise from the nitrogen gas inlet tube, and the changes in pressure and temperature over time in the reaction vessel were measured. After 5 hours, the pressure in the reaction vessel decreased rapidly. Thereafter, while maintaining the reaction vessel at 80 ° C., under conditions of 0.5 MPa or less, a mixture of EO1111g was gradually added dropwise from the nitrogen gas inlet tube. After the addition was completed, the reaction was carried out at 80°C for 1 hour, and the reaction mixture was extracted from the reaction layer and filtered to remove solids, thereby obtaining a liquid product of the monomer of formula (b) in which 2 moles of PO were added to HPMA and then 7 moles of EO were added. When the molecular weight distribution was confirmed by GPC, it was found that b / w f was 1.75. The structure is 1 Confirmed by H NMR.
[0077] Synthesis of MAEM Represented by (d) [Synthesis Example 1-3] 9.28 g of 2-acetamidoethanol and 100 mL of dehydrated dichloromethane were added to a 250 mL flask equipped with a thermometer, a gas inlet tube, a stirrer, and a dropping funnel. The atmosphere in the flask was thoroughly purged with argon gas, and then 13.15 g of triethylamine was added. The system was then cooled to -15°C, and 11.29 g of methacrylic acid chloride was slowly added dropwise from the dropping funnel while monitoring the thermometer so that the temperature remained at approximately -9°C. After the addition was complete, the mixture was stirred at room temperature for 3 hours. The reaction mixture was filtered to remove the precipitate, and the filtrate was washed successively with water, a saturated aqueous solution of sodium bicarbonate, and a saturated aqueous solution of sodium chloride. After drying with sodium sulfate, the mixture was concentrated under reduced pressure using a rotary evaporator to obtain an oily product. Further purification was performed by silica gel chromatography using hexane and ethyl acetate as eluents, and the example compound 2-(acetylamino)ethyl methacrylate was obtained. The structure is 1The product was confirmed by H NMR. 2-(acetylamino)ethyl methacrylate (MAEM) was synthesized according to the procedure described in JP 2017-160380 A.
[0078] <Copolymer (P)> In the examples, copolymers 1 to 6 shown below were used as working polymers.
[0079] MPC: 2-methacryloyloxyethyl phosphorylcholine (product of NOF Corporation) Compound I: polyethylene glycol-polypropylene glycol monomethacrylate (random adduct of PO and EO (PO / EO = 3.3 / 5.7 mol), p≒10, w b / w f = 1.59, synthesized in Synthesis Example 1-1) Compound II: polyethylene glycol-polypropylene glycol monomethacrylate (block adduct of PO and EO (PO / EO = 2.0 / 7.0 mol), p ≒ 10, w b / w f = 1.75, synthesized in Synthesis Example 1-2) MAEM: 2-(acetylamino)ethyl methacrylate (synthesized in Synthesis Example 1-3) NVP: N-vinylpyrrolidone (product of Fujifilm Wako Pure Chemical Industries, Ltd.) The formulas of the compounds used are summarized in Table 1.
[0080] <Measurement of weight-average molecular weight> 1 mg of the obtained copolymer was dissolved in 1 g of mobile phase and measured. Other measurement conditions were as follows: Column: SB-802.5 HQ + SB-806MN HQ + SB-G Mobile phase: 20 mM phosphate buffer (pH 7.0) Standard substance: polyethylene glycol / oxide Measuring instrument: HLC-8320GPC (manufactured by Tosoh Corporation) Method for calculating weight-average molecular weight: molecular weight calculation program (EcoSEC Date Analysis) Flow rate: 0.5 mL per minute Injection volume: 100 μL Column oven: 45°C Measurement time: 90 minutes
[0081] <Polymerization of Copolymers for Examples> [Example 1-1] 0.90 g of MPC and 4.18 g of Compound I (synthesized in Synthesis Example 1-1) were dissolved in 14.4 g of water and 14.4 g of ethanol, and the solution was placed in a 100 mL four-neck flask. Nitrogen was blown in at a flow rate of 0.2 L / min for 30 minutes (MPC: Compound I = 30:70 (molar ratio)). 0.51 g of Perbutyl (registered trademark) ND (PB-ND, manufactured by NOF Corporation) was added at 55°C and stirred for 3 hours, after which the temperature was raised to 75°C and polymerization reaction was carried out for an additional 2 hours. After completion of the reaction, 14.4 g of water was added, and distillation was carried out for 1 hour. The resulting reaction solution was purified by dialysis to obtain a polymer solution (Copolymer 1). The weight average molecular weight was confirmed by GPC to be 32,100.
[0082] [Example 1-2] 2.20 g of MPC and 2.92 g of Compound I were dissolved in 14.5 g of water and 14.5 g of ethanol, and the solution was placed in a 100 mL four-neck flask. Nitrogen was blown in at a flow rate of 0.2 L / min for 30 minutes (MPC: Compound I = 60:40 (molar ratio)). 0.51 g of PB-ND was added at 55°C and stirred for 3 hours, then the temperature was raised to 75°C and polymerization reaction was carried out for an additional 2 hours. After completion of the reaction, 14.5 g of water was added, and distillation was carried out for 1 hour. The resulting reaction solution was purified by dialysis to obtain a polymer solution (Copolymer 2). The weight average molecular weight was confirmed by GPC to be 150,500.
[0083] Example 1-3 1.70 g of MPC, 5.64 g of Compound I, and 0.66 g of MAEM (synthesized in Synthesis Example 1-3) were dissolved in 16.0 g of water and 16.0 g of ethanol, and the solution was placed in a 100 mL four-neck flask. Nitrogen was blown in at a flow rate of 0.2 L / min for 30 minutes (MPC: Compound I: MAEM = 30:50:20 (molar ratio)). 0.40 g of PB-ND was added at 55°C and stirred for 3 hours, then the temperature was raised to 75°C and polymerization reaction was carried out for an additional 2 hours. After completion of the reaction, 16.0 g of water was added, and distillation was carried out for 1 hour. The resulting reaction solution was purified by dialysis to obtain a polymer solution (Copolymer 3). The weight average molecular weight was confirmed by GPC to be 190,500.
[0084] [Example 1-4] 2.20 g of MPC, 2.63 g of Compound I, and 0.33 g of NVP were dissolved in 14.6 g of water and 14.6 g of ethanol, and the solution was placed in a 100 mL four-neck flask. Nitrogen was blown in at a flow rate of 0.2 L / min for 30 minutes (MPC: Compound I: NVP = 50:30:20 (molar ratio)). 0.52 g of PB-ND was added at 55°C and stirred for 3 hours, then the temperature was raised to 75°C and polymerization reaction was carried out for an additional 2 hours. After completion of the reaction, 14.6 g of water was added, and distillation was carried out for 1 hour. The resulting reaction solution was purified by dialysis to obtain a polymer solution (Copolymer 4). The weight average molecular weight was confirmed by GPC to be 100,500.
[0085] [Example 1-5] 0.50 g of MPC, 4.31 g of Compound I, and 0.39 g of MAEM were dissolved in 14.7 g of water and 14.7 g of ethanol, and the solution was placed in a 100 mL four-neck flask. Nitrogen was blown in at a flow rate of 0.2 L / min for 30 minutes (MPC: Compound I: MAEM = 15:65:20 (molar ratio)). 0.52 g of PB-ND was added at 55°C and stirred for 3 hours, then the temperature was raised to 75°C and polymerization reaction was carried out for an additional 2 hours. After completion of the reaction, 14.7 g of water was added, and distillation was carried out for 1 hour. The resulting reaction solution was purified by dialysis to obtain a polymer solution (Copolymer 5). The weight average molecular weight was confirmed by GPC to be 29,500.
[0086] Example 1-6 0.90 g of MPC and 4.22 g of Compound II (synthesized in Synthesis Example 1-2) were dissolved in 14.5 g of water and 14.5 g of ethanol, and the solution was placed in a 100 mL four-neck flask. Nitrogen was blown in at a flow rate of 0.2 L / min for 30 minutes (MPC: Compound II = 30:70 (molar ratio)). 0.51 g of PB-ND was added at 55°C and stirred for 3 hours, then the temperature was raised to 75°C and polymerization reaction was carried out for an additional 2 hours. After completion of the reaction, 14.5 g of water was added, and distillation was carried out for 1 hour. The resulting reaction solution was purified by dialysis to obtain a polymer solution (Copolymer 6). The weight-average molecular weight was confirmed by GPC to be 98,500.
[0087] <Comparative Copolymers> In the comparative examples, the following homopolymers 1 and 2, copolymers 7 and 8, and PVP K30 (polyvinylpyrrolidone K30) were used as comparative polymers.
[0088] <Polymerization of Comparative Copolymers> [Comparative Example 1-1] 5.00 g of MPC was dissolved in 14.2 g of water and 14.2 g of ethanol, and the solution was placed in a 100 mL four-neck flask. Nitrogen was blown in at a flow rate of 0.2 L / min for 30 minutes. 0.50 g of PB-ND was added at 55°C and stirred for 3 hours. The temperature was then raised to 75°C and the polymerization reaction was carried out for an additional 2 hours. After completion of the reaction, 14.2 g of water was added, and distillation was carried out for 1 hour. The resulting reaction solution was purified by dialysis to obtain a polymer solution (homocopolymer 1). The weight average molecular weight was confirmed by GPC to be 300,000.
[0089] [Comparative Example 1-2] 5.10 g of compound I was dissolved in 14.5 g of water and 14.5 g of ethanol, and the solution was placed in a 100 mL four-neck flask. Nitrogen was blown in at a flow rate of 0.2 L / min for 30 minutes. 0.51 g of PB-ND was added at 55°C and stirred for 3 hours, after which the temperature was raised to 75°C and the polymerization reaction was carried out for an additional 2 hours. After completion of the reaction, 14.5 g of water was added, and distillation was carried out for 1 hour. The resulting reaction solution was purified by dialysis to obtain a polymer solution (homocopolymer 2). The weight average molecular weight was confirmed by GPC and was 20,000.
[0090] Comparative Example 1-3: 3.30 g of MPC and 1.91 g of MAEM were dissolved in 14.8 g of water and 14.8 g of ethanol, and the solution was placed in a 100 mL four-neck flask. Nitrogen was blown in at a flow rate of 0.2 L / min for 30 minutes (MPC:MAEM = 50:50 (molar ratio)). 0.52 g of PB-ND was added at 55°C and stirred for 3 hours, after which the temperature was raised to 75°C and polymerization reaction was carried out for an additional 2 hours. After completion of the reaction, 14.8 g of water was added, and distillation was carried out for 1 hour. The resulting reaction solution was purified by dialysis to obtain a polymer solution (Copolymer 7). The weight-average molecular weight was confirmed by GPC to be 53,600.
[0091] Comparative Example 1-4: 3.50 g of MPC and 1.54 g of 2-hydroxyethyl methacrylate (HEMA) were dissolved in 14.3 g of water and 14.3 g of ethanol, and the solution was placed in a 100 mL four-neck flask. Nitrogen was blown in at a flow rate of 0.2 L / min for 30 minutes (MPC:HEMA = 50:50 (molar ratio)). 0.50 g of PB-ND was added at 55°C and stirred for 3 hours, after which the temperature was raised to 75°C and polymerization reaction was carried out for an additional 2 hours. After completion of the reaction, 14.3 g of water was added, and distillation was carried out for 1 hour. The resulting reaction solution was purified by dialysis to obtain a polymer solution (Copolymer 8). The weight-average molecular weight was confirmed by GPC to be 356,000.
[0092] <Test contact lenses used in evaluation> Lens A: One Day Fine UV Plus, a soft contact lens (product of Seed Co., Ltd.) Lens B: AQUAFORCE UV, a soft contact lens (product of Aimi Co., Ltd.)
[0093] <Preparation of physiological saline solution> Physiological saline solution was prepared with reference to the literature (ISO 18369-3:2017, Ophthalmic Optics - Contact Lenses Part 3: Measurement Methods.) 8.3 g of sodium chloride, 5.993 g of sodium hydrogen phosphate dodecahydrate, and 0.528 g of sodium dihydrogen phosphate dihydrate were weighed out, dissolved in water to make 1000 mL, and filtered to obtain physiological saline solution.
[0094] <Preparation of Treatment Solution for Soft Contact Lenses> <Example 2-1> A solution of copolymer 1 was dissolved in a predetermined amount of physiological saline to prepare a 5 wt % polymer solution shown in Table 2 below. 2 g of the polymer solution was then mixed with 98 g of physiological saline to prepare the contact lens treatment solution shown in Table 2 below. Test contact lenses treated with this contact lens treatment solution were evaluated for hydrophilicity, lubricity, and durability. The evaluation results are shown in Table 2 below.
[0095] Examples 2-2 to 2-9: Test contact lenses were treated with contact lens treatment solutions prepared in the same manner as in Example 1, except that the polymers shown in Tables 2 and 3 below were used, and the hydrophilicity, lubricity, and durability of the treated contact lenses were evaluated. The evaluation results are shown in Tables 2 and 3 below.
[0096] Comparative Examples 2-1 to 2-5: Test contact lenses were treated with contact lens treatment solutions prepared in the same manner as in Example 1, except that the polymers and PVP K30 shown in Table 4 below were used, and the hydrophilicity, lubricity, and durability of the treated contact lenses were evaluated. The evaluation results are shown in Table 4 below.
[0097] <Hydrophilicity Evaluation> In the Examples and Comparative Examples, the surface hydrophilicity of soft contact lenses was evaluated according to the following procedure. ○ Evaluation of surface hydrophilicity simulating the start of soft contact lens wear (1) 10 mL of physiological saline was added to a 15 mL conical tube, and five test contact lenses removed from blister packs were immersed therein, followed by shaking at 50 rpm using a roller mixer at room temperature for 6 hours. (2) The test contact lenses were removed and sealed in 10 mL glass vials containing 5 mL of soft contact lens treatment solution prepared for each lens. (3) The lenses were sterilized at 121°C for 20 minutes. (4) The test contact lenses were removed from the glass vials, and the time (BUT) until the water film on the lens surface disappeared was measured with a stopwatch, and the results were evaluated according to the following criteria.
[0098] ○ Evaluation of surface hydrophilicity of soft contact lenses simulating the end of wear (1) 10 mL of saline was added to a 15 mL conical tube, and five test contact lenses removed from blister packs were immersed in the solution. The solution was then shaken at room temperature for 6 hours using a roller mixer at a rotation speed of 50 rpm. (2) The test contact lenses were removed and sealed in 10 mL glass vials containing 5 mL of soft contact lens treatment solution prepared for each lens. (3) The lenses were sterilized at 121°C for 20 minutes. (4) 2 mL of saline was added to one well of a 12-well plate, and one test contact lens removed from the glass vial was immersed in the solution. The lenses were then shaken at 80 rpm for 4 hours at 37°C using a shaker. (5) The test contact lenses were removed from the 12-well plate, and the time until the water film on the lens surface disappeared (BUT) was measured using a stopwatch and evaluated according to the following criteria.
[0099] The evaluation, which assumes the end of wear, takes into account the actual tear volume and blinking frequency throughout the day and assumes the condition of the contact lenses after wearing them all day (12 hours of continuous wear).
[0100] The evaluation criteria are as follows: 4 points: 20 seconds or more 3 points: 15 seconds or more 2 points: 10 seconds or more but less than 15 seconds 1 point: 5 seconds or more but less than 10 seconds 0 point: Less than 5 seconds
[0101] <Lubricity Evaluation> In the Examples and Comparative Examples, the lubricity of contact lenses was evaluated according to the following procedure. Lubricity Evaluation Simulating the Initial Wear of Soft Contact Lenses (1) 10 mL of saline was added to a 15 mL conical tube, and five test contact lenses removed from blister packs were immersed therein. The solution was shaken at room temperature for 6 hours at a rotation speed of 50 rpm using a roller mixer. (2) The test contact lenses were removed and sealed in 10 mL glass vials containing 5 mL of soft contact lens treatment solution prepared for each lens. (3) The lenses were sterilized at 121°C for 20 minutes. (4) The test contact lenses were removed from the glass vials, and the coefficient of friction in saline was measured using a Nanotribometer NTR3 (probe material: polypropylene, load: 2 mN, travel distance: 1.00 mm, speed: 0.1 mm / s), and the results were evaluated according to the following criteria.
[0102] Lubricity evaluation simulating the end of soft contact lens wear (1) 10 mL of saline was added to a 15 mL conical tube, and five test contact lenses removed from blister packs were immersed in the solution. The solution was then shaken at room temperature for 6 hours using a roller mixer at a rotation speed of 50 rpm. (2) The test contact lenses were removed and sealed in 10 mL glass vials containing 5 mL of the soft contact lens treatment solution prepared for each lens. (3) The lenses were sterilized at 121°C for 20 minutes. (4) 2 mL of saline was added to one well of a 12-well plate, and one test contact lens removed from the glass vial was immersed in the solution. The solution was then shaken at 80 rpm for 4 hours at 37°C using a shaker. (5) The test contact lenses were removed from the 12-well plate, and the friction coefficient was measured using a nanotribometer NTR3 (probe material: polypropylene, load: 2 mN, movement distance: 1.00 mm, speed: 0.1 mm / s), and evaluated according to the following criteria.
[0103] The evaluation, which assumes the end of wear, takes into account the actual tear volume and blinking frequency throughout the day and assumes the condition of the contact lenses after wearing them all day (12 hours of continuous wear).
[0104] The evaluation criteria are as follows: 4 points: less than 0.30 3 points: 0.30 or more and less than 0.5 2 points: 0.50 or more and less than 1.0 1 point: 1.0 or more and less than 1.5 0 point: 1.5 or more
[0105] <Evaluation of Durability> In the Examples and Comparative Examples, the evaluation of durability was based on the evaluation results of hydrophilicity and lubricity and was evaluated according to the following criteria: ◎: The scores for the assumed time at the start of wearing and the assumed time at the end of wearing were the same in both evaluations ○: The scores for the assumed time at the start of wearing and the assumed time at the end of wearing were reduced by 1 point in either evaluation, or the scores for the assumed time at the start of wearing and the assumed time at the end of wearing were reduced by 1 point in both evaluations △: The scores for the assumed time at the start of wearing and the assumed time at the end of wearing were reduced by 2 points in either evaluation ×: The scores for the assumed time at the start of wearing and the assumed time at the end of wearing were reduced by 2 points in both evaluations, or the scores for the assumed time at the start of wearing and the assumed time at the end of wearing were reduced by 3 points or more in either evaluation
[0106] <Evaluation of Wearing Comfort> The wearing comfort of the Examples and Comparative Examples was evaluated according to the following criteria based on the evaluation results of hydrophilicity and lubricity assumed at the end of wearing. Excellent wearing comfort: Hydrophilicity: 4, Lubricity: 4 Hydrophilicity: 4, Lubricity: 3 Hydrophilicity: 3, Lubricity: 4 Good wearing comfort: Hydrophilicity: 3, Lubricity: 3 : Hydrophilicity: 2, Lubricity: 3 : Hydrophilicity: 3, Lubricity: 2 : Hydrophilicity: 2, Lubricity: 2 Unsatisfactory wearing comfort: Other than the above
[0107]
[0108]
[0109]
[0110] <Evaluation> The contact lens treatment solutions of Examples 2-2, 2-4, 2-5, and 2-9 were able to impart excellent hydrophilicity and excellent lubricity to the surface of soft contact lenses at the assumed start and end of wear, and these properties were also very well maintained. That is, the contact lens treatment solutions of Examples 2-2, 2-4, 2-5, and 2-9 were able to impart excellent wearing comfort to soft contact lenses for long periods of time due to their excellent hydrophilicity and lubricity, which are maintained for a long period of time. The contact lens treatment solutions of Examples 2-7 and 2-8 were able to impart excellent hydrophilicity and lubricity to the surface of soft contact lenses for the assumed start and end of wear, and these properties were also very well maintained. That is, the contact lens treatment solutions of Examples 2-7 and 2-8 were able to impart excellent wearing comfort to soft contact lenses for long periods of time due to their excellent hydrophilicity and lubricity, which are maintained for a long period of time. The contact lens treatment solutions of Examples 2-1, 2-3, and 2-6 were able to impart good hydrophilicity and good lubricity to the surface of soft contact lenses at the estimated start and end of wear, and these properties were also well-maintained. That is, the contact lens treatment solutions of Examples 2-1, 2-3, and 2-6 were able to impart good wearing comfort to soft contact lenses for a long period of time due to their good hydrophilicity and lubricity and their persistence. The contact lens treatment solution of Comparative Example 1-1 had good hydrophilicity at the estimated start of wear compared to each Example, but was significantly inferior in persistence. The contact lens treatment solution of Comparative Example 1-2 had good hydrophilicity at the estimated start of wear, but insufficient lubricity and insufficient wearing comfort. The contact lens treatment solution of Comparative Example 1-3 had good hydrophilicity at the estimated start of wear, but insufficient lubricity, and insufficient persistence and wearing comfort. The contact lens treatment solution of Comparative Example 1-4 had good hydrophilicity as expected at the start of use, but insufficient lubricity and was significantly inferior in durability. The contact lens treatment solution of Comparative Example 1-5 had good wearing comfort as expected at the start of use, but was significantly inferior in durability.
[0111] This application claims priority based on Japanese Application No. 2023-053617 filed on March 29, 2023, and the contents of the specification, claims and drawings of that application are incorporated herein by reference.
[0112] By using the soft contact lens treatment solution of the present invention on soft contact lenses, it is possible to impart excellent wearing comfort to the soft contact lenses all day (for a long period of time).
Claims
1. Having structural units represented by the following formulas (A) and (B), the molar ratio n of the structural unit represented by the following formula (A) to the entire copolymer (P) A is 10 to 80 mol %, and the molar ratio n B and a weight average molecular weight of 10,000 to 2,000,000. [In the above formula (A) and formula (B), R 1 and R 2 Each of X in formula (A) independently represents a hydrogen atom or a methyl group. 3 , where R 3 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 4 O represents an oxyalkylene group having 2 to 4 carbon atoms; R 4 O contains at least two kinds of oxyalkylene groups having different carbon numbers, and the addition form thereof may be either block or random, and p represents the average number of moles of the oxyalkylene groups added and is a number from 4 to 100.
2. The copolymer (P) has a constitutional unit represented by the following formula (C) or (D), and the molar ratio n of the constitutional unit represented by the following formula (C) or (D) to the entire copolymer (P): C and n D The copolymer according to claim 1, wherein the sum of is greater than 0 mol % and not more than 50 mol %. [In the above formula (C), R 5 is H or a methylene group, R 6 is an alkyl group having 1 to 5 carbon atoms, or R 5 is a methylene group, the end is R 5 In formula (D), R is an alkylene group having 1 to 5 carbon atoms and bonded to the 7 is a hydrogen atom or a methyl group, and Y is O or NR 10 , where R 10 is H or an alkyl group having 1 to 4 carbon atoms, and when Y is O, E 1 is a structure represented by formula (E), and Y is NR 10 In the case of E 1 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, or a structure represented by formula (E). In formula (E), R 8 is H or an alkyl group having 1 to 4 carbon atoms, R 9 is a hydrogen atom or an alkyl group having 1 to 18 carbon atoms.
3. The copolymer according to claim 1 or 2, wherein the structural unit (A) is a structural unit derived from 2-(methacryloyloxy)ethyl 2-(trimethylammonio)ethyl phosphate.
4. A contact lens treatment solution containing 0.001 w / v % or more and 5.0 w / v % or less of the copolymer (P) according to any one of claims 1 to 3.
Citation Information
Patent Citations
Multifunctional bionic polymer, its preparation method and application
CN102796224A
Bondable blood-friendly polymer as well as production method and application thereof
CN103193927A
Insulin secretomotor and endothelin-1 production-suppressing substance
JP2005008607A
Detection kit and examination method
JP2013228383A
Copolymer, bioactive material immobilization polymer for catching biomolecules, coating composition, and article
JP2018070716A