Optical element and optical device

The optical element, comprising specific λ/4 plates and liquid crystal layers, addresses the challenge of converting circularly polarized light in AR glasses by efficiently converting light within a specific wavelength range with opposite rotation, minimizing refraction angle dependence.

WO2024203584A1PCT designated stage expired Publication Date: 2024-10-03FUJIFILM CORP

Patent Information

Application Number
PCT/JP2024/010683
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-19
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing optical elements for AR glasses lack a configuration that can efficiently convert circularly polarized light in a specific wavelength range into circularly polarized light with the opposite rotation direction, while minimizing wavelength dependence of refraction angles.

Method used

An optical element comprising a first λ/4 plate, an optical laminate, and a second λ/4 plate, where the optical laminate includes a first liquid crystal layer with a twist angle of 16.5 to 36.5° and a second liquid crystal layer with a twist angle of 68.6 to 88.6°, both layers having refractive index differences that produce a product within specific ranges, allowing for the conversion of circularly polarized light in a specific wavelength range.

Benefits of technology

The optical element effectively converts circularly polarized light in a specific wavelength range into circularly polarized light with the opposite rotation direction, while maintaining minimal wavelength dependence of refraction angles, enhancing the performance of AR glasses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010683_03102024_PF_FP_ABST
    Figure JP2024010683_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing an optical element having a novel configuration capable of converting only circularly polarized light in a specific wavelength region into circularly polarized light in a reverse turning direction. An optical element according to the present invention comprises a first λ / 4 plate, an optical laminate, and a second λ / 4 plate in this order. The optical laminate has, in a thickness direction, two or more liquid crystal layer pairs each comprising a first liquid crystal layer formed by fixing a liquid crystal compound which is twist-aligned in the thickness direction, and a second liquid crystal layer formed by fixing a liquid crystal compound which is twist-aligned in the thickness direction and the twist direction of which is a direction opposite to the twist direction of the liquid crystal compound in the first liquid crystal layer. In the liquid crystal layer pair, the alignment direction of the liquid crystal compound on the surface on the second liquid crystal layer side of the first liquid crystal layer, and the alignment direction of the liquid crystal compound on the surface on the first liquid layer side of the second liquid crystal layer are parallel, and the twist angle of the liquid crystal compound in the first liquid crystal layer and the twist angle of the liquid crystal compound in the second liquid crystal layer are equal.
Need to check novelty before this filing date? Find Prior Art

Description

optical elements, optical devices

[0001] The present invention relates to an optical element and an optical device using the optical element.

[0002] In recent years, AR (Augmented Reality) glasses that display virtual images and various information superimposed on an actual scene have been put to practical use. AR glasses are also called smart glasses, head-mounted displays (HMDs), AR glasses, and the like.

[0003] Patent Document 1 discloses an optical element in which the refraction angle has little wavelength dependency, and for example, red light, green light, and blue light incident from the same direction can be refracted and emitted in almost the same direction, and it is described that this optical element is applicable to AR glass. The optical element described in Patent Document 1 claims that the wavelength dependency of the refraction angle can be reduced by using a wavelength-selective retardation layer (optical element) in combination with multiple optically anisotropic layers. It is described that the wavelength-selective retardation layer (optical element) has the function of converting circularly polarized light in a specific wavelength range into circularly polarized light with an opposite rotation direction.

[0004] International Publication No. 2019 / 131918

[0005] The above-mentioned patent documents describe wavelength-selective retardation layers (optical elements) as described above, but there has been a demand for optical elements with novel configurations different from these. Therefore, an object of the present invention is to provide an optical element with a novel configuration that can convert only circularly polarized light in a specific wavelength range into circularly polarized light with the opposite rotation direction. Another object of the present invention is to provide an optical element using the above-mentioned optical element.

[0006] The present inventors have conducted extensive research to solve the above problems and have completed the present invention. That is, they have found that the above problems can be solved by the following configuration.

[0007] [1] An optical element having, in this order, a first λ / 4 plate, an optical laminate, and a second λ / 4 plate, wherein the optical laminate has two or more liquid crystal layer pairs in the thickness direction, each pair consisting of a first liquid crystal layer formed by fixing a liquid crystal compound that is twisted in the thickness direction, and a second liquid crystal layer formed by fixing a liquid crystal compound that is twisted in the thickness direction, the second liquid crystal layer having a twisted liquid crystal compound that is twisted in the thickness direction, the twist direction of the liquid crystal compound being opposite to the twist direction of the liquid crystal compound in the first liquid crystal layer, wherein in the liquid crystal layer pairs, the orientation direction of the liquid crystal compound on the surface of the first liquid crystal layer facing the second liquid crystal layer is parallel to the orientation direction of the liquid crystal compound on the surface of the second liquid crystal layer facing the first liquid crystal layer, and the twist angle of the liquid crystal compound in the first liquid crystal layer is equal to the twist angle of the liquid crystal compound in the second liquid crystal layer. [2] The optical element according to [1], wherein either a rod-shaped liquid crystal compound or a discotic liquid crystal compound is contained in the liquid crystal compound in the first liquid crystal layer, and the other is contained in the liquid crystal compound in the second liquid crystal layer. [3] The optical element according to [1] or [2], wherein at least one of the first λ / 4 plate and the second λ / 4 plate is a laminate comprising a liquid crystal layer A formed by fixing a liquid crystal compound that is twisted in the thickness direction, and a liquid crystal layer B formed by fixing a liquid crystal compound that is twisted in the thickness direction. [4] The optical element according to [1] or [2], wherein the twist angle of the liquid crystal compound in the liquid crystal layer A is 16.5 to 36.5°, and the refractive index difference Δn of the liquid crystal layer A is A and the thickness d of the liquid crystal layer A A The product Δn A d A is 252 to 312 nm, the twist angle of the liquid crystal compound in the liquid crystal layer B is 68.6 to 88.6°, and the refractive index difference Δn B and the thickness d of the liquid crystal layer B B The product Δn B d B[5] The optical element according to [3], wherein the liquid crystal layer A is disposed on the optical laminate side, and the alignment direction of the liquid crystal compound on the liquid crystal layer A side surface of the optical laminate is parallel to the alignment direction of the liquid crystal compound on the liquid crystal layer A side surface of the liquid crystal layer A. [6] The optical element according to any one of [3] to [5], wherein the alignment direction of the liquid crystal compound on the liquid crystal layer B side surface of the liquid crystal layer A is parallel to the alignment direction of the liquid crystal compound on the liquid crystal layer A side surface of the liquid crystal layer B. [7] An optical element comprising: a plurality of optically anisotropic layers formed using a composition containing a liquid crystal compound, the layers having a liquid crystal orientation pattern in which the orientation of the optical axis derived from the liquid crystal compound changes while continuously rotating along at least one direction in a plane; and the optical element according to any one of [1] to [6], which is disposed between at least a pair of adjacent two optically anisotropic layers in the plurality of optically anisotropic layers; and wherein, in the liquid crystal orientation pattern of the optically anisotropic layers, when the length of a 180° rotation of the orientation of the optical axis derived from the liquid crystal compound in the one direction in which the orientation of the optical axis derived from the liquid crystal compound changes while continuously rotating is defined as one period, at least one of the optically anisotropic layers has a length of one period different from that of the other optically anisotropic layers.

[0008] The present invention provides an optical element having a novel configuration that can convert only circularly polarized light in a specific wavelength range into circularly polarized light with the opposite rotation direction. The present invention also provides an optical element using the optical element.

[0009] 16 is a diagram conceptually showing an example of the optical element of the present invention. FIG. 17 is a graph for explaining the optical element of the present invention. FIG. 18 is a graph for explaining the optical element of the present invention. FIG. 19 is a graph for explaining the optical element of the present invention. FIG. 20 is a diagram conceptually showing another example of the optical element of the present invention. FIG. 21 is a graph for explaining the optical element shown in FIG. 4. FIG. 22 is a diagram conceptually showing an example of the optical element of the present invention. FIG. 23 is a diagram conceptually showing the optically anisotropic layer of the optical element shown in FIG. 6. FIG. 24 is a plan view of the optically anisotropic layer of the optical element shown in FIG. 6. FIG. 25 is a conceptual diagram showing the function of the optically anisotropic layer of the optical element shown in FIG. 6. FIG. 26 is a conceptual diagram showing the function of the optical element shown in FIG. 6. FIG. 27 is a diagram conceptually showing another example of the optical element of the present invention. FIG. 28 is a conceptual diagram showing the function of the optical element shown in FIG. 12. FIG. 29 is a diagram conceptually showing an example of an exposure apparatus for exposing an alignment film of the optical element shown in FIG. 6. FIG. 29 is a plan view of another example of the optically anisotropic layer of the optical element of the present invention. FIG. 29 is a diagram conceptually showing an example of an exposure apparatus for exposing an alignment film that forms the optically anisotropic layer shown in FIG. 16. 1 is a diagram conceptually showing an example of AR glasses using an example of the optical element of the present invention, and FIG. 2 is a diagram conceptually showing another example of the optically anisotropic layer of the optical element of the present invention.

[0010] The present invention will be described in detail below. The following description of the components may be based on representative embodiments of the present invention, but the present invention is not limited to such embodiments.

[0011] The meaning of each description in this specification is as follows: In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits.

[0012] Re(λ) and Rth(λ) respectively represent the in-plane retardation and the retardation in the thickness direction at a wavelength λ. Re(λ), Rth(λ), and Δnd are measured using an AXOSCAN (manufactured by AXOMETRICS).

[0013] In this specification, "visible light" refers to 380 nm to 780 nm. Unless otherwise specified, the measurement wavelength is 550 nm. In this specification, angular relationships (e.g., "perpendicular," "parallel," and specific angles) are intended to include the range of error acceptable in the technical field to which the present invention pertains. Specifically, this means a range of less than ±10° from the exact angle, and the error from the exact angle is preferably 5° or less, and more preferably 3° or less. The figures shown below are conceptual diagrams for explaining the present invention, and the positional relationship, size, thickness, shape, etc. of each component may differ from the actual ones.

[0014] <Optical Element> The optical element of the present invention includes a first λ / 4 plate, an optical laminate, and a second λ / 4 plate, in this order. The optical laminate includes two or more liquid crystal layer pairs in the thickness direction, each pair consisting of a first liquid crystal layer having a liquid crystal compound twisted and aligned in the thickness direction, and a second liquid crystal layer having a liquid crystal compound twisted and aligned in the thickness direction, the second liquid crystal layer having a liquid crystal compound twisted and aligned in the thickness direction, the twist direction of the liquid crystal compound being opposite to the twist direction of the liquid crystal compound in the first liquid crystal layer. In the liquid crystal layer pair, the alignment direction of the liquid crystal compound on the surface of the first liquid crystal layer facing the second liquid crystal layer is parallel to the alignment direction of the liquid crystal compound on the surface of the second liquid crystal layer facing the first liquid crystal layer. The twist angle of the liquid crystal compound in the first liquid crystal layer is equal to the twist angle of the liquid crystal compound in the second liquid crystal layer.

[0015] FIG. 1 conceptually illustrates an example of an optical element of the present invention. The optical element 210 shown in FIG. 1 includes a first λ / 4 plate 212, a second λ / 4 plate 214, and a liquid crystal polarization interference element 216. The liquid crystal polarization interference element 216 is disposed between the first λ / 4 plate 212 and the second λ / 4 plate 214. The liquid crystal polarization interference element 216 corresponds to the optical laminate in the optical element of the present invention. The liquid crystal polarization interference element 216 is an optical element that acts as a λ / 2 retardation plate for light in a specific wavelength range (specific wavelength) and does not act as a retardation layer for other light. Therefore, the optical element 210 shown in FIG. 1 can convert only circularly polarized light in a specific wavelength range into circularly polarized light with the opposite rotation direction. Circularly polarized light outside the specific wavelength range is transmitted without changing its rotation direction. In other words, the optical element 210 of the present invention functions as a wavelength-selective retardation layer for circularly polarized light.

[0016] The first λ / 4 plate 212 and the second λ / 4 plate 214 are plates that have the function of converting linearly polarized light of a specific wavelength into circularly polarized light (or circularly polarized light into linearly polarized light). More specifically, they are plates that exhibit an in-plane retardation of λ / 4 (or an odd multiple thereof) at a specific wavelength λ nm. There are no particular limitations on the first λ / 4 plate 212 and the second λ / 4 plate 214, and known λ / 4 plates can be used. The first λ / 4 plate 212 and the second λ / 4 plate 214 will be described in detail later.

[0017] In the illustrated optical element 210, a liquid crystal polarization interference element 216 is disposed between the first λ / 4 plate 212 and the second λ / 4 plate 214. Note that in FIG. 1 , the first λ / 4 plate 212 and the second λ / 4 plate 214 are spaced apart from the liquid crystal polarization interference element 216. However, the present invention is not limited to this, and the first λ / 4 plate 212 and the second λ / 4 plate 214 may be stacked in contact with the liquid crystal polarization interference element 216. Furthermore, when the first λ / 4 plate 212 and the second λ / 4 plate 214 are in contact with the liquid crystal polarization interference element 216, they may be adhered to each other, if necessary, with an adhesive that is transparent to transmitted light, such as an OCA (Optical Clear Adhesive) or an acrylic adhesive.

[0018] The liquid crystal polarization interference element 216 is formed by stacking an even number of liquid crystal layers, each of which has a liquid crystal compound 218 twisted in the thickness direction. The liquid crystal compound 218 is a rod-shaped liquid crystal compound. Specifically, the liquid crystal polarization interference element 216 is formed by alternately stacking a first liquid crystal layer 220, each of which has a liquid crystal compound 218 twisted in the thickness direction, and a second liquid crystal layer 224, each of which has a liquid crystal compound 218 twisted in the thickness direction, and in which the twist direction of the liquid crystal compound 218 is opposite to that of the first liquid crystal layer 220. The liquid crystal polarization interference element 216 has a configuration in which two or more liquid crystal layer pairs 226 are stacked in the thickness direction, each pair consisting of a first liquid crystal layer 220 and a second liquid crystal layer 224. Therefore, the total number of first liquid crystal layers 220 and second liquid crystal layers 224 is an even number.

[0019] In one liquid crystal layer set 226, the alignment direction of the liquid crystal compound 218 on the surface of the first liquid crystal layer 220 facing the second liquid crystal layer 224 is parallel to the alignment direction of the liquid crystal compound 218 on the surface of the second liquid crystal layer 224 facing the first liquid crystal layer 220. That is, in one liquid crystal layer set 226, the alignment directions of the liquid crystal compound 218 at the interface between the first liquid crystal layer 220 and the second liquid crystal layer 224 are parallel.

[0020] In one liquid crystal layer set 226, the alignment direction of the liquid crystal compound 218 on the surface of the first liquid crystal layer 220 facing the second liquid crystal layer 224 and the alignment direction of the liquid crystal compound 218 on the surface of the second liquid crystal layer 224 facing the first liquid crystal layer 220 can be detected by obliquely cutting the liquid crystal polarization interference element 216 and analyzing the alignment direction of the liquid crystal on the cross-sectional surface. This method is described in detail in "Depth-Dependent Determination of Molecular Orientation for WV-Film" by Yohei Takahashi et al. (FMC8-3, IDW'04, pp. 651-654).

[0021] Furthermore, in one liquid crystal layer set 226, the twist angle of the liquid crystal compound 218 in the thickness direction in the first liquid crystal layer 220 is equal to the twist angle of the liquid crystal compound 218 in the thickness direction in the second liquid crystal layer 224. As described above, the twist directions of the liquid crystal compound 218 in the thickness direction are opposite to those in the first liquid crystal layer 220 and the second liquid crystal layer 224. That is, for example, when the twist angle of the liquid crystal compound 218 in the first liquid crystal layer 220 is φ [°], the twist angle of the liquid crystal compound 218 in the first liquid crystal layer 220 is −φ [°]. Therefore, in one liquid crystal layer set 226, the liquid crystal compound 218 is twisted to a certain angle in the thickness direction in the first liquid crystal layer 220, and then twists back to its original angle in the second liquid crystal layer 224. For example, if the twist angle of the liquid crystal compound 218 in the thickness direction is 30°, the liquid crystal compound 218 twists from 0° to 30° in the first liquid crystal layer 220, and then twists from 30° back to 0° in the second liquid crystal layer 224.

[0022] In this example, the twist angle of the liquid crystal compound is, for example, positive (+) when it is clockwise and negative (-) when it is counterclockwise, with the direction of the transmission axis of the first λ / 4 plate 212 being 0°. That is, the absolute values ​​of the twist angles of the first liquid crystal layer 220 and the second liquid crystal layer 224 are the same.

[0023] As described above, the liquid crystal polarization interference element 216 has liquid crystal compounds 218 (rod-shaped liquid crystal compounds) twisted in the thickness direction, and further has first and second liquid crystal layers 220 and 224 alternately stacked in the thickness direction, with the liquid crystal compounds 218 oriented parallel to each other at their interfaces, the liquid crystal compounds 218 twisted in opposite directions, and the absolute value of the twist angle being equal. That is, light passing through the liquid crystal polarization interference element 216 is repeatedly and alternately influenced by a slow axis rotating by a predetermined angle in one direction and a slow axis rotating by a predetermined angle in the opposite direction. For example, if the absolute value of the twist angle of the liquid crystal compounds 218 is 30°, the light passing through the liquid crystal polarization interference element 216 is repeatedly and alternately influenced by a slow axis rotating from 0° to 30° and a slow axis rotating from 30° to 0°. Therefore, in the liquid crystal polarization interference element 216, by setting Δnd of the first liquid crystal layer 220 and the second liquid crystal layer 224 according to the wavelength range in which the optical element 210 converts circularly polarized light into circularly polarized light with the opposite rotation direction, and further adjusting the twist angle of the liquid crystal compound in the first liquid crystal layer 220 and the second liquid crystal layer 224 according to the total number of layers of the first liquid crystal layer 220 and the second liquid crystal layer 224, it is possible to form a liquid crystal polarization interference element 216 that acts as a λ / 2 retardation plate for light in a specific wavelength range but does not act as a retardation plate for other light, i.e., does not sense retardation.

[0024] The number of liquid crystal layer pairs 226 that the liquid crystal polarization interference element 216 has can be detected by cutting the liquid crystal polarization interference element 216 obliquely and analyzing the orientation direction of the liquid crystal on the surface of the cross section. This method is described in detail in the above-mentioned publication by Yohei Takahashi et al. Furthermore, the change in the twist direction of the liquid crystal can be determined based on the difference in components in the depth direction of the element, as it is due to the difference in the chiral agent, using a time-of-flight secondary ion mass spectrometry (TOF-SIMS) device (TOF.SIMS5, manufactured by ION-TOF).

[0025] In Δnd of the first liquid crystal layer 220 and the second liquid crystal layer 224 constituting the liquid crystal polarization interference element 216, Δn is the birefringence of the liquid crystal compound 218 constituting the first liquid crystal layer 220 and the second liquid crystal layer 224. Furthermore, d is the thickness of the first liquid crystal layer 220 and the second liquid crystal layer 224. Δn can also be measured using an AxoScan manufactured by Axometrics, Inc. In the present invention, Δnd of the first liquid crystal layer 220 and the second liquid crystal layer 224 is equal. As described above, the liquid crystal polarization interference element 216 acts as a λ / 2 retarder only for light in a specific wavelength range. Accordingly, Δnd of the first liquid crystal layer 220 and the second liquid crystal layer 224 is set to a wavelength at which the liquid crystal polarization interference element 216 is expected to act as a λ / 2 retarder, i.e., half the center wavelength (half wavelength) of the wavelength range at which the optical element 210 is expected to convert circularly polarized light into circularly polarized light with the opposite rotation direction. For example, assuming that the wavelength at which the liquid crystal polarization interference element 216 acts as a λ / 2 retarder, i.e., the central wavelength of the wavelength range in which the optical element 210 converts circularly polarized light into circularly polarized light with the opposite rotation direction, is 550 nm, Δnd of the first liquid crystal layer 220 and the second liquid crystal layer 224 is set to 275 nm. Note that Δnd of the first liquid crystal layer 220 and the second liquid crystal layer 224 may have an error of about ±10% with respect to half the central wavelength of the wavelength range in which the optical element 210 converts circularly polarized light into circularly polarized light with the opposite rotation direction.

[0026] On the other hand, the twist angle of the liquid crystal compound 218 in the first liquid crystal layer 220 and the second liquid crystal layer 224 constituting the liquid crystal polarization interference element 216 is set by simulation to be an optimal twist angle at which the liquid crystal polarization interference element 216 acts as a λ / 2 retardation plate, depending on the central wavelength of the wavelength range in which the optical element 210 is assumed to convert circularly polarized light into circularly polarized light having the opposite rotation direction, and the total number N of layers of the first liquid crystal layer 220 and the second liquid crystal layer 224. This simulation can be performed using a general optical simulation means, or it can also be calculated using LCD Master 1D (manufactured by Shintech Co., Ltd., Ver. 9.8.0.0).

[0027] Here, according to a simulation by the inventors, the twist angle φ of the liquid crystal compound 218 in the first liquid crystal layer 220 and the second liquid crystal layer 224 with respect to the total number of layers N of the first liquid crystal layer 220 and the second liquid crystal layer 224 is as follows: when the number of stacked layers N is 2 (one liquid crystal layer set), the twist angle φ is 63.6°; when the number of stacked layers N is 4 (two liquid crystal layer sets), the twist angle φ is 35.5°; when the number of stacked layers N is 6 (three liquid crystal layer sets), the twist angle φ is 23.6°; when the number of stacked layers N is 8 (four liquid crystal layer sets), the twist angle φ is 17.7°; when the number of stacked layers N is 10 (five liquid crystal layer sets), the twist angle φ is 14.1°; and when the number of stacked layers N is 12 (six liquid crystal layer sets), the twist angle φ is 11.8°. When the number of stacked layers N is 14 (7 liquid crystal layer sets), the optimum twist angle φ is 10.1°, and when the number of stacked layers N is 16 (8 liquid crystal layer sets), the optimum twist angle φ is 8.8°.

[0028] As conceptually shown in FIG. 2, fitting this result (solid line) with an approximate curve (dashed line) gives the following equation: φ=129.05×N -0.961 Accordingly, in the present invention, the twist angle ±φ [°] of the liquid crystal compound 218 in the first liquid crystal layer 220 and the second liquid crystal layer 224, which corresponds to the total number N of stacked layers of the first liquid crystal layer 220 and the second liquid crystal layer 224, is given by 0.9×(129.05×N -0.961 )≦|φ|≦1.1×(129.05×N -0.961 ) and |φ|=129.05×N -0.961 It is more preferable to set it as follows.

[0029] The absolute values ​​of the twist angles of the liquid crystal compound 218 in the first liquid crystal layer 220 and the second liquid crystal layer 224 are not limited to being the same, and may have an error of ±10% or less of the absolute value of the twist angle. However, it is preferable that this error is small, and it is most preferable that the absolute values ​​of the twist angles of the liquid crystal compound 218 in the first liquid crystal layer 220 and the second liquid crystal layer 224 are the same.

[0030] The twist angle of the liquid crystal compound 218 in the first liquid crystal layer 220 and the second liquid crystal layer 224 constituting the liquid crystal polarization interference element 216 can be detected by obliquely cutting the liquid crystal polarization interference element 216 and analyzing the orientation direction of the liquid crystal on the surface of the cross section. This method is described in detail in the above-mentioned document by Yohei Takahashi et al. The twist angle of the liquid crystal compound 218 can also be measured using AxoScan (manufactured by Axometrics) by a separation measurement means that assumes a model into which parameters have been input.

[0031] There are no limitations on the thickness d of the first liquid crystal layer 220 and the second liquid crystal layer 224, and the thickness may be set appropriately depending on the liquid crystal compound 218 used so that Δnd is half the central wavelength of the wavelength range in which the optical element 210 converts circularly polarized light into circularly polarized light with the opposite rotation direction. The thickness d of the first liquid crystal layer 220 and the second liquid crystal layer 224 is preferably 1 to 5 μm, and more preferably 1 to 3 μm. The first liquid crystal layer 220 and the second liquid crystal layer 224 are typically formed using the same liquid crystal compound 218. The Δnd of the first liquid crystal layer 220 and the second liquid crystal layer 224 are also equal. Therefore, the thicknesses of the first liquid crystal layer 220 and the second liquid crystal layer 224 are equal.

[0032] There are no other limitations on the total number N of layers of the first liquid crystal layers 220 and the second liquid crystal layers 224, as long as the number of liquid crystal layer sets 226 is two or more, i.e., four or more layers, and the number is an even number. The total number N of layers of the first liquid crystal layers 220 and the second liquid crystal layers 224 is preferably 4 to 30 layers, more preferably 4 to 20 layers, and even more preferably 4 to 10 layers.

[0033] In the optical element 210 of the present invention, the greater the total number N of layers of the first liquid crystal layer 220 and the second liquid crystal layer 224, i.e., the greater the number of liquid crystal layer pairs 226, the narrower the wavelength range in which the liquid crystal polarization interference element 216 acts as a λ / 2 retardation layer. Therefore, in the optical element 210 of the present invention, the greater the total number N of layers of the first liquid crystal layer 220 and the second liquid crystal layer 224, the narrower the half-width of the wavelength range of light that converts circularly polarized light into circularly polarized light with the opposite rotation direction. In other words, the greater the total number N of layers of the first liquid crystal layer 220 and the second liquid crystal layer 224, the narrower the wavelength range in which the optical element 210 converts circularly polarized light into circularly polarized light with the opposite rotation direction. Therefore, the total number N of layers of the first liquid crystal layer 220 and the second liquid crystal layer 224, i.e., the number of liquid crystal layer sets 226, can be selected appropriately depending on the width of the wavelength range required for the optical element 210, with a smaller number of layers selected when a wide band is preferred and a larger number of layers selected when a narrow band is required.

[0034] Such a liquid crystal polarization interference element 216 may be fabricated by a known method, for example, by a coating method using a liquid crystal composition for forming the first liquid crystal layer 220 and the second liquid crystal layer 224.

[0035] First, an alignment film oriented in one direction is formed on an appropriately selected support. The alignment film may be a known alignment film, such as a rubbed film made of an organic compound such as a polymer, an obliquely evaporated film of an inorganic compound, a film having a microgroove, a film formed by accumulating LB (Langmuir-Blodgett) films made of organic compounds such as ω-tricosanoic acid, dioctadecylmethylammonium chloride, and methyl stearate by the Langmuir-Blodgett method, or a film formed by applying an alignment film-forming coating liquid containing a photoalignment material to the surface of a support, drying the coating, and exposing the coating using a polarizer such as a wire grid polarizer.

[0036] Meanwhile, a composition (liquid crystal composition) for forming the first liquid crystal layer 220 and a composition for forming the second liquid crystal layer 224 are prepared, each containing a liquid crystal compound and a chiral agent capable of inducing a twisted alignment of the liquid crystal compound in the thickness direction. The first liquid crystal layer 220 and the second liquid crystal layer 224 have opposite twist directions of the liquid crystal compound 218 in the thickness direction, but the twist direction of the liquid crystal compound in the thickness direction can be selected by selecting the chiral agent. Furthermore, the twist angle of the liquid crystal compound 218 in the thickness direction can be adjusted by adjusting the amount of chiral agent added.

[0037] The solvent for preparing the composition is not limited and can be appropriately selected depending on the purpose, but organic solvents are preferred.The organic solvent is not limited and can be appropriately selected depending on the purpose, and examples thereof include ketones, alkyl halides, amides, sulfoxides, heterocyclic compounds, hydrocarbons, esters, and ethers.These may be used alone or in combination of two or more.Among these, ketones are preferred when considering the burden on the environment.

[0038] A composition for forming the first liquid crystal layer 220 is applied to the surface of the formed alignment film to align the liquid crystal compound 218, and then dried, and if necessary, the composition is hardened by irradiation with ultraviolet light or the like to form the first liquid crystal layer 220.

[0039] Next, a composition for forming the second liquid crystal layer 224 is applied to the surface of the formed first liquid crystal layer 220, dried, and optionally cured by ultraviolet irradiation or the like to form the second liquid crystal layer 224, thereby forming a first liquid crystal layer set. When a liquid crystal layer is formed on top of the first liquid crystal layer by a coating method, the upper liquid crystal layer follows the alignment of the liquid crystal compound on the surface of the lower liquid crystal layer. Therefore, at the interface between the first liquid crystal layer 220 and the second liquid crystal layer 224, the alignment direction of the liquid crystal compound 218 in the first liquid crystal layer 220 and the alignment direction of the liquid crystal compound 218 in the second liquid crystal layer 224 are parallel (match).

[0040] Next, a composition for forming the first liquid crystal layer 220 is applied to the surface of the formed second liquid crystal layer 224, dried, and optionally cured by ultraviolet irradiation or the like to form the first liquid crystal layer 220. In the liquid crystal polarization interference element 216 constituting the optical element 210 of the present invention, the twist of the liquid crystal compound 218 in the thickness direction in the first liquid crystal layer 220 and the twist of the liquid crystal compound 218 in the thickness direction in the second liquid crystal layer have the same twist angle but opposite twist directions. Therefore, if the orientation angle of the liquid crystal compound 218 at the interface between the first liquid crystal layer 220 formed on the surface of the alignment film and the alignment film is set to 0°, the orientation angle of the liquid crystal compound 218 on the upper surface of the second liquid crystal layer 224 also returns to 0°. Furthermore, as described above, when a liquid crystal layer is formed on a liquid crystal layer by a coating method, the liquid crystal compound near the interface with the lower layer of the upper liquid crystal layer follows the orientation of the liquid crystal compound on the surface of the lower liquid crystal layer. Therefore, at the interface between the second liquid crystal layer 224 and the first liquid crystal layer 220, the alignment direction of the liquid crystal compound 218 in the second liquid crystal layer 224 and the alignment direction of the liquid crystal compound 218 in the first liquid crystal layer 220 are parallel at 0°.

[0041] Next, a second liquid crystal layer 224 is similarly formed on the surface of the formed first liquid crystal layer 220, then a first liquid crystal layer 220 is similarly formed on the surface of the formed second liquid crystal layer 224, and then a second liquid crystal layer 224 is similarly formed on the surface of the formed first liquid crystal layer 220. This process is repeated the same number of times as the number of liquid crystal layers to be formed, i.e., the number of liquid crystal layer pairs to be formed, to produce a liquid crystal polarization interference element 216. Furthermore, for example, the angle between the alignment direction of the liquid crystal compound 218 in the first formed first liquid crystal layer 220 and the in-plane slow axis of the first λ / 4 plate 212 is set to 45°, and further, the second λ / 4 plate 214 is arranged so that the in-plane slow axis of the first λ / 4 plate 212 and the in-plane slow axis of the second λ / 4 plate 212 are perpendicular to each other, and the liquid crystal polarization interference element 216 is sandwiched between them in the thickness direction (stacking direction), thereby producing the optical element 210 shown in FIG. In the above, the angle between the orientation direction of the liquid crystal compound 218 in the first liquid crystal layer 220 formed initially and the in-plane slow axis of the first λ / 4 plate 212 is set to 45°, but the angle may be 45°±15°, and 45°±10° is preferred.

[0042] In the liquid crystal polarization interference element 216 of the optical element 210 of the present invention, the first liquid crystal layer 220 and the second liquid crystal layer 224 are not limited to those formed by a coating method and directly laminated as described above. That is, the liquid crystal polarization interference element 216 may be formed by preparing the first liquid crystal layer 220 and the second liquid crystal layer 224 in sheet form, alternately laminating them, and attaching them with an adhesive that is transparent to transmitted light, such as OCA or an acrylic adhesive. However, in terms of the transmittance of transmitted light, the first liquid crystal layer 220 and the second liquid crystal layer 224 that are directly laminated by a coating method and do not have an adhesive layer or the like are preferred.

[0043] In the optical element 210 (liquid crystal polarization interference element 216) of the present invention, the liquid crystal compound 218 (rod-shaped liquid crystal compound) is not limited, and various known liquid crystal compounds can be used. Preferred rod-shaped liquid crystal compounds include azomethines, azoxys, cyanobiphenyls, cyanophenyl esters, benzoates, cyclohexanecarboxylic acid phenyl esters, cyanophenylcyclohexanes, cyano-substituted phenylpyrimidines, alkoxy-substituted phenylpyrimidines, phenyldioxanes, tolanes, and alkenylcyclohexylbenzonitriles. In addition to the above-mentioned low-molecular-weight liquid crystal molecules, polymeric liquid crystal molecules can also be used.

[0044] In the first liquid crystal layer 220 and the second liquid crystal layer 224, it is more preferable to fix the alignment of the rod-shaped liquid crystal compound by polymerization. Examples of the polymerizable rod-shaped liquid crystal compound include those described in Makromol. Chem. , Vol. 190, p. 2255 (1989), Advanced Materials Vol. 5, p. 107 (1993), U.S. Patent Nos. 4,683,327, 5,622,648, 5,770,107, WO 95 / 22586, 95 / 24455, 97 / 00600, 98 / 23580, 98 / 52905, JP-A-1-272551, JP-A-6-16616, JP-A-7-110469, JP-A-11-80081, and compounds described in Japanese Patent Application No. 2001-64627 can be used. Furthermore, as the rod-shaped liquid crystal compound, for example, those described in JP-A-11-513019 and JP-A-2007-279688 can also be preferably used.

[0045] As described above, the chiral agent has the function of inducing a helical orientation of a liquid crystal compound in the thickness direction. The chiral agent can be selected according to the purpose, since the helical twist direction or helical pitch induced by the chiral agent varies depending on the compound.

[0046] The chiral agent is not particularly limited, and known compounds (for example, those described in Liquid Crystal Device Handbook, Chapter 3, Section 4-3, Chiral Agents for TN (Twisted Nematic) and STN (Super Twisted Nematic), p. 199, edited by the 142nd Committee of the Japan Society for the Promotion of Science, 1989), isosorbide (a chiral agent having an isosorbide structure), isomannide derivatives, and the like can be used. Furthermore, chiral agents that undergo back isomerization, dimerization, or isomerization and dimerization, etc., upon irradiation with light, and thereby reduce helical twisting power (HTP), can also be suitably used.

[0047] Chiral agents generally contain an asymmetric carbon atom, but axially asymmetric or planarly asymmetric compounds without an asymmetric carbon atom can also be used as chiral agents. Examples of axially asymmetric or planarly asymmetric compounds include binaphthyl, helicene, paracyclophane, and derivatives thereof. The chiral agent may have a polymerizable group. When both the chiral agent and the liquid crystal compound have a polymerizable group, a polymer having a repeating unit derived from the polymerizable liquid crystal compound and a repeating unit derived from the chiral agent can be formed by polymerization of the polymerizable chiral agent and the polymerizable liquid crystal compound. In this embodiment, the polymerizable group of the polymerizable chiral agent is preferably the same type of group as the polymerizable group of the polymerizable liquid crystal compound. Therefore, the polymerizable group of the chiral agent is preferably an unsaturated polymerizable group, an epoxy group, or an aziridinyl group, more preferably an unsaturated polymerizable group, and even more preferably an ethylenically unsaturated polymerizable group. The chiral agent may also be a liquid crystal compound.

[0048] When the chiral agent has a photoisomerizable group, a pattern of a desired reflection wavelength corresponding to the emission wavelength can be formed by irradiating the chiral agent with actinic rays or the like through a photomask after coating and alignment. The photoisomerizable group is preferably an isomerization site of a compound exhibiting photochromic properties, an azo group, an azoxy group, or a cinnamoyl group. Specific compounds that can be used include those described in JP-A-2002-080478, JP-A-2002-080851, JP-A-2002-179668, JP-A-2002-179669, JP-A-2002-179670, JP-A-2002-179681, JP-A-2002-179682, JP-A-2002-338575, JP-A-2002-338668, JP-A-2003-313189, and JP-A-2003-313292.

[0049] The twist angle of the liquid crystal compound 218 in the thickness direction varies depending on the amount of chiral dopant added. Therefore, by selecting the chiral dopant and appropriately setting the amount added, the twist direction and twist angle of the liquid crystal compound 218 in the first liquid crystal layer 220 and the second liquid crystal layer 224 can be set as desired.

[0050] In addition to the liquid crystal compound and the chiral agent, the composition for forming the first liquid crystal layer 220 and the second liquid crystal layer 224 may contain, if necessary, a polymerization initiator, a leveling agent, a crosslinking agent, a surfactant, etc.

[0051] In the optical element 210 shown in FIG. 1 , all of the first liquid crystal layers 220 are the same, and all of the second liquid crystal layers 224 are the same. That is, in the optical element 210 shown in FIG. 1 , all of the first liquid crystal layers 220 have the same Δnd and the same twist angle of the liquid crystal compound 218, and all of the second liquid crystal layers 224 have the same Δnd and the same twist angle of the liquid crystal compound 218. However, the present invention is not limited to this, and the Δnd of the liquid crystal layer and the twist angle of the liquid crystal compound 218 may have a distribution in the thickness direction. That is, in the optical element of the present invention, as long as the Δnd of the first and second liquid crystal layers is the same, the twist directions of the liquid crystal compound 218 are opposite, and the twist angles (absolute values ​​of the twist angles) are the same, the Δnd and the twist angles of the liquid crystal compound 218 may differ between pairs of liquid crystal layers.

[0052] As an example, a configuration is exemplified in which the liquid crystal layer pair at the center in the thickness direction (stacking direction) and the liquid crystal layer pairs on both sides in the thickness direction have different Δnd of the liquid crystal layer and the twist angle of the liquid crystal compound 218. Specifically, compared to the liquid crystal layer of the liquid crystal layer pair at the center in the thickness direction, the Δnd of the liquid crystal layer of the liquid crystal layer pairs on both sides in the thickness direction may be made larger and the twist angle of the liquid crystal compound 218 may be made smaller. As an example, if the optical element (liquid crystal polarization interference element) has eight liquid crystal layers, i.e., four liquid crystal layer sets, in the first liquid crystal layer set, Δnd of the first liquid crystal layer (first layer) is set to Δnd1, the twist angle of the liquid crystal compound is set to φ1, Δnd of the second liquid crystal layer (second layer) is set to Δnd1, and the twist angle of the liquid crystal compound is set to -φ1, in the second liquid crystal layer set, Δnd of the first liquid crystal layer (third layer) is set to Δnd2 smaller than Δnd1, and the twist angle of the liquid crystal compound is set to φ2 larger than φ1, Δnd of the second liquid crystal layer (fourth layer) is set to Δnd2, and the twist angle of the liquid crystal compound is set to -φ2, In the third liquid crystal layer set, the Δnd of the first liquid crystal layer (fifth layer) is Δnd2, the twist angle of the liquid crystal compound is φ2, the Δnd of the second liquid crystal layer (sixth layer) is Δnd2, and the twist angle of the liquid crystal compound is −φ2; and in the fourth liquid crystal layer set, the Δnd of the first liquid crystal layer (seventh layer) is Δnd1, the twist angle of the liquid crystal compound is φ1, the Δnd of the second liquid crystal layer (eighth layer) is Δnd1, and the twist angle of the liquid crystal compound is −φ1.

[0053] As described above, the liquid crystal polarization interference element acts as a λ / 2 retarder for light in a specific wavelength range of interest, but does not act as a retarder for other light. On the other hand, when linear polarizers arranged in a crossed Nicol configuration are provided above and below the liquid crystal polarization interference element, the liquid crystal polarization interference element functions as a bandpass filter centered on a specific wavelength range, as conceptually shown in FIG. 3 . That is, in the above embodiment, the liquid crystal polarization interference element functions as a bandpass filter having a high transmittance in a specific wavelength range and a low transmittance in other wavelength ranges. However, transmission wavelength ranges called side lobes, as indicated by arrows S in the figure, may occur at wavelengths shorter and longer than the specific wavelength range of interest, sandwiching the specific wavelength range. That is, the liquid crystal polarization interference element may also generate polarization components caused by the function of the λ / 2 retarder in wavelength ranges other than the specific wavelength range. In response to this, as described above, the side lobes can be reduced by increasing the Δnd of the liquid crystal layers of the liquid crystal layer pairs on both sides of the thickness direction and reducing the twist angle of the liquid crystal compound 218 compared to the liquid crystal layer of the central liquid crystal layer pair in the thickness direction. That is, the polarized light component generated by the function of the λ / 2 retardation plate can be reduced.

[0054] The Δnd of the liquid crystal layer can be adjusted by, for example, changing the thickness of the liquid crystal layer, but it can also be adjusted by changing the liquid crystal compound used. The twist angle of the liquid crystal compound can be adjusted by changing the type and / or amount of the chiral dopant added.

[0055] In this configuration, the Δnd of the liquid crystal layer of each pair of liquid crystal layers on both sides in the thickness direction is larger than that of the liquid crystal layer of the central pair of liquid crystal layers in the thickness direction, and the twist angle of the liquid crystal compound 218 is smaller. In other words, the number of the central liquid crystal layer, which has the Δnd of the liquid crystal layer larger and the twist angle of the liquid crystal compound 218 smaller than that of the pair of liquid crystal layers on both sides, is not limited, and may be appropriately set according to the number of liquid crystal layers (liquid crystal layer pairs) of the liquid crystal polarization interference element of the optical element. In addition, the Δnd of the liquid crystal layer of each pair of liquid crystal layers on both sides in the thickness direction and the twist angle of the liquid crystal compound 218, as well as the Δnd of the liquid crystal layer of the central pair of liquid crystal layers in the thickness direction and the twist angle of the liquid crystal compound 218, may be set by simulation to be optimal Δnd and twist angle that can reduce side lobes when the liquid crystal polarization interference element acts as a λ / 2 retarder and is used as a band-pass filter as described above. It is preferable to control the change in the twist angle of the liquid crystal compound 218 from both sides toward the center in the stacking direction (thickness direction) and the thickness-wise distribution of Δnd of the liquid crystal layer of the liquid crystal layer set as smoothly and precisely as possible.

[0056] In the optical element 210 shown in FIG. 1 , the liquid crystal compound 218 in each liquid crystal layer is a rod-shaped liquid crystal compound, and the liquid crystal layer is composed solely of the rod-shaped liquid crystal compound. However, the present invention is not limited to this. That is, in the optical element of the present invention, the liquid crystal layer may contain a discotic liquid crystal compound in addition to the liquid crystal compound 218, as in the first liquid crystal layer 232 and the second liquid crystal layer 234 of the optical element 230 shown in FIG. 4 . That is, either a rod-shaped liquid crystal compound or a discotic liquid crystal compound may be contained in the liquid crystal compound in the first liquid crystal layer 232, and the other may be contained in the liquid crystal compound in the second liquid crystal layer 234. In the following description, the liquid crystal compound 218 will also be referred to as the rod-shaped liquid crystal compound 218 to clearly distinguish it from the discotic liquid crystal compound 240. In addition, in the optical element 230 shown in FIG. 4 , the same components are denoted by the same reference numerals, and the following description will mainly focus on the different components.

[0057] 4, the first liquid crystal layer 232 and the second liquid crystal layer 234 are also formed by fixing rod-shaped liquid crystal compounds 218 and discotic liquid crystal compounds 240 that are twisted in the thickness direction. Also in the optical element 230, the twist directions of the liquid crystal compounds are opposite to those of the first liquid crystal layer 232 and the second liquid crystal layer 234, but the twist angles of the liquid crystal compounds are the same. That is, the total twist angles of the rod-shaped liquid crystal compounds 218 and the discotic liquid crystal compounds 240 in the first liquid crystal layer 232 and the second liquid crystal layer 234 are in the relationship of "φ" and "-φ", as in the previous example. Furthermore, also in the optical element 230, the alignment directions of the liquid crystal compounds are parallel at the interface between the first liquid crystal layer 232 and the second liquid crystal layer 234.

[0058] 4 , the first liquid crystal layer 232 has, in the thickness direction from bottom to top in the figure, first rod-shaped liquid crystal compounds 218 twisted in the thickness direction, and then discotic liquid crystal compounds 240 twisted in the thickness direction. Conversely, the second liquid crystal layer 234 on top of it has, in the thickness direction from bottom to top in the figure, first discotic liquid crystal compounds 240 twisted in the thickness direction, and then rod-shaped liquid crystal compounds 218 twisted in the thickness direction. The twisted orientation directions of the liquid crystal compounds in the first liquid crystal layer 232 and the second liquid crystal layer 234 are opposite to each other. The optical element 230 also includes a liquid crystal polarization interference element 246 in which such first liquid crystal layers 232 and second liquid crystal layers 234 are alternately stacked, and the liquid crystal polarization interference element 246 includes two or more liquid crystal layer pairs each consisting of a first liquid crystal layer 232 and a second liquid crystal layer 234. In the example shown in Fig. 4, in the liquid crystal layer pair 236, the first liquid crystal layer 232 is arranged in the order of "rod-shaped liquid crystal compound / discotic liquid crystal compound" from bottom to top in the thickness direction of the figure, and the second liquid crystal layer 234 is arranged in the order of "discotic liquid crystal compound / rod-shaped liquid crystal compound," but the present invention is not limited to this. For example, in the optical element of the present invention, the first liquid crystal layer may be arranged in the order of "rod-shaped liquid crystal compound / discotic liquid crystal compound" from bottom to top in the thickness direction of the figure, and the second liquid crystal layer may be arranged in the order of "rod-shaped liquid crystal compound / discotic liquid crystal compound" from bottom to top in the thickness direction of the figure. Furthermore, the number, order, and thickness of the regions consisting of rod-shaped liquid crystal compounds 218 and the regions consisting of discotic liquid crystal compounds 240 may be changed as appropriate, provided that the Δnd of each liquid crystal layer and the sum of the twist angles of the liquid crystal compounds do not change.

[0059] As conceptually shown in Figure 5, in a bandpass filter using the above-mentioned liquid crystal polarization interference element 216, when light is incident from an oblique direction, a wavelength shift occurs in which the transmission wavelength range moves toward shorter wavelengths. In contrast, as in the liquid crystal polarization interference element 246, the first liquid crystal layer 232 and the second liquid crystal layer 234 have a region made of rod-shaped liquid crystal compounds 218 and a region made of discotic liquid crystal compounds 240, thereby reducing the retardation (Rth) in the thickness direction of the first liquid crystal layer 232 and the second liquid crystal layer 234, thereby suppressing wavelength shift (coloring) when light is incident from an oblique direction. In other words, even if circularly polarized light is incident from a direction tilted from the normal direction to the surface of the optical element 230, only circularly polarized light in the intended specific wavelength range can be converted into circularly polarized light with the opposite rotation direction.

[0060] When the first liquid crystal layer 232 and the second liquid crystal layer 234 are composed of a region consisting of rod-shaped liquid crystal compounds 218 and a region consisting of discotic liquid crystal compounds 240, there is no limitation on the ratio of the thicknesses of the region consisting of rod-shaped liquid crystal compounds 218 and the region consisting of discotic liquid crystal compounds 240. Here, when the first liquid crystal layer 232 and the second liquid crystal layer 234 are composed of a region consisting of rod-shaped liquid crystal compounds 218 and a region consisting of discotic liquid crystal compounds 240, it is preferable that the Δnd of the liquid crystal layer be shared equally between the region consisting of rod-shaped liquid crystal compounds 218 and the region consisting of discotic liquid crystal compounds 240, depending on the Δn of the liquid crystal compound used. Furthermore, it is preferable that the Δn of the rod-shaped liquid crystal compounds 218 and the discotic liquid crystal compounds 240 have the same value from the viewpoint of reducing interfacial reflection, but different Δn values ​​may also be used.

[0061] The liquid crystal polarization interference element 246 comprising a liquid crystal layer having such a region consisting of the rod-shaped liquid crystal compound 218 and a region consisting of the discotic liquid crystal compound 240 can also be formed by a coating method using a composition for forming the region consisting of the rod-shaped liquid crystal compound 218 in the first liquid crystal layer 232, a composition for forming the region consisting of the discotic liquid crystal compound 240 in the first liquid crystal layer 232, a composition for forming the region consisting of the discotic liquid crystal compound 240 in the second liquid crystal layer 234, and a composition for forming the region consisting of the rod-shaped liquid crystal compound 218 in the second liquid crystal layer 234, as described above. In both cases where a region consisting of the discotic liquid crystal compound 240 is formed on the region consisting of the rod-shaped liquid crystal compound 218, and where a region consisting of the rod-shaped liquid crystal compound 218 is formed on the region consisting of the discotic liquid crystal compound 240, the liquid crystal compound in the region formed above follows the alignment direction (longitudinal direction) of the liquid crystal compound in the region below, as described above. Therefore, in a liquid crystal layer having a region made of rod-shaped liquid crystal compounds 218 and a region made of discotic liquid crystal compounds 240, the liquid crystal compounds are twisted and oriented continuously in the thickness direction within a single liquid crystal layer, and the orientation directions of the liquid crystal compounds at the interface between the first liquid crystal layer 232 and the second liquid crystal layer 234 are parallel.

[0062] As described above, in the present invention, not only can liquid crystal layers (regions) be directly laminated by a coating method, but also sheet-like liquid crystal layers can be laminated and attached with an OCA, etc. Also, in the present invention, a liquid crystal layer set consisting of the first liquid crystal layer 232 and the second liquid crystal layer 234 can be formed at one time by coating a composition containing the discotic liquid crystal compound 240 and the rod-shaped liquid crystal compound 218.

[0063] In the present invention, when the first liquid crystal layer 232 and the second liquid crystal layer 234 have a region made of the discotic liquid crystal compound 240, there is no limitation on the discotic liquid crystal compound to be used, and various known compounds can be used. As the discotic liquid crystal compound, for example, those described in JP-A-2007-108732 and JP-A-2010-244038 can be preferably used. When a discotic liquid crystal compound is used in the liquid crystal layer, the discotic liquid crystal compound 240 stands up in the thickness direction in the liquid crystal layer as shown in FIG. 4 , and the optical axis derived from the liquid crystal compound is defined as an axis perpendicular to the disc surface, i.e., a so-called fast axis.

[0064] 4 each have one region made of rod-shaped liquid crystal compound 218 and one region made of discotic liquid crystal compound 240, the present invention is not limited thereto. That is, in the present invention, when the first liquid crystal layer and the second liquid crystal layer each have a region made of rod-shaped liquid crystal compound and a region made of discotic liquid crystal compound, one liquid crystal layer may have a plurality of regions made of rod-shaped liquid crystal compound and / or a plurality of regions made of discotic liquid crystal compound.

[0065] The twist angle and twist direction of the liquid crystal compound in the first liquid crystal layer 232 and the second liquid crystal layer 234 constituting the liquid crystal polarization interference element 246 can be detected by obliquely cutting the liquid crystal polarization interference element 246 and analyzing the alignment direction of the liquid crystal on the surface of the cross section. This method is described in detail in the above-mentioned document by Yohei Takahashi et al.

[0066] In the optical element of the present invention, the first liquid crystal layer and the second liquid crystal layer may contain an infrared absorbing dye. By containing the infrared absorbing dye in the first liquid crystal layer and the second liquid crystal layer, the liquid crystal wavelength dispersion in the liquid crystal layers can be made to be a strong forward dispersion. As a result, the wavelength range of light over which the liquid crystal polarization interference element acts as a λ / 2 wave plate can be narrowed. In other words, by adding an infrared absorbing dye to the first liquid crystal layer and the second liquid crystal layer to make the liquid crystal wavelength dispersion in the liquid crystal layers a strong forward dispersion, an optical element can be obtained that converts circularly polarized light into circularly polarized light with an opposite rotation direction, with a narrower wavelength range.

[0067] As the infrared absorbing dye, various infrared absorbing dyes can be used that can reduce the difference in refractive index between the x and y directions by being oriented in the same direction as the liquid crystal compound. There are no particular limitations on the infrared absorbing dye, as long as it absorbs infrared light (e.g., light with a wavelength of 700 to 900 m). Among these, dichroic dyes are preferred. A dichroic dye refers to a dye that has different absorbance in the long axis direction and the short axis direction of the molecule. Examples of infrared absorbing dyes that can be used include diketopyrrolopyrrole dyes, diimmonium dyes, phthalocyanine dyes, naphthalocyanine dyes, azo dyes, polymethine dyes, anthraquinone dyes, pyrylium dyes, squarylium dyes, triphenylmethane dyes, cyanine dyes, and aminium dyes. Metal complex dyes and boron complex dyes can also be used as the infrared absorbing dye. Infrared absorbing dyes are described in detail in WO 2019 / 044859.

[0068] There is no restriction on the amount of infrared absorbing dye added to the first liquid crystal layer and the second liquid crystal layer, and it may be set appropriately depending on the width of the wavelength range required for the optical element to convert circularly polarized light into circularly polarized light with the opposite rotation direction.

[0069] In the optical element of the present invention, the first and second liquid crystal layers may contain a liquid crystal elastomer. The first and second liquid crystal layers containing a liquid crystal elastomer may be formed using a liquid crystal elastomer, or may be formed of a normal liquid crystal compound other than an elastomer and then contain a liquid crystal elastomer.

[0070] In this way, by including a liquid crystal elastomer in the first and second liquid crystal layers, the first and second liquid crystal layers can be made elastic, and the thickness of the liquid crystal layer can be changed by stretching or shrinking the optical element in the plane direction. By changing the thickness of the liquid crystal layer, the Δnd of the liquid crystal layer can be changed. As a result, it is possible to change the wavelength range of light that converts circularly polarized light into circularly polarized light with the opposite rotation direction in the optical element. In other words, by including a liquid crystal elastomer in the first and second liquid crystal layers, the wavelength range can be changed by stretching and shrinking the liquid crystal layer, i.e., the optical element, enabling active wavelength control in the optical element.

[0071] There are no limitations on the liquid crystal elastomer, and various known ones can be used. As an example of the liquid crystal elastomer, a liquid crystal elastomer prepared from a liquid crystal monomer, a chiral agent, a crosslinking agent, and a plasticizer, as described in JP 2020-131638 A, can be used. This provides the liquid crystal elastomer with mechanical properties and rubber elasticity, enabling it to deform in response to the external force required for active wavelength control.

[0072] In addition, when the first and second liquid crystal layers are formed from a normal liquid crystal compound that is not an elastomer and a liquid crystal elastomer is added to impart elasticity, there is no restriction on the amount of liquid crystal elastomer added, and it can be set appropriately depending on the required elasticity, i.e., the control range of the wavelength range that converts circularly polarized light into circularly polarized light with the opposite rotation direction.

[0073] Such an optical element of the present invention can be used at any wavelength, i.e., the optical element of the present invention can be used for any electromagnetic wave, such as ultraviolet light, visible light, infrared light, terahertz waves, and millimeter waves.

[0074] The optical elements of the present invention have been described in detail above, but the present invention is not limited to the above examples, and various improvements and modifications may be made without departing from the spirit of the present invention.

[0075] [First λ / 4 Plate and Second λ / 4 Plate] The optical element of the present invention has a first λ / 4 plate and a second λ / 4 plate. As described above, the first λ / 4 plate and the second λ / 4 plate are plates that have the function of converting linearly polarized light of a specific wavelength into circularly polarized light (or circularly polarized light into linearly polarized light). The first λ / 4 plate 212 and the second λ / 4 plate 214 are not particularly limited, and known λ / 4 plates can be used. The in-plane retardation Re(550) at a wavelength of 550 nm of the first λ / 4 plate 212 and the second λ / 4 plate 214 is preferably 100 to 200 nm, more preferably 120 to 160 nm, and even more preferably 130 to 150 nm.

[0076] The λ / 4 plate may consist of one layer or two or more layers. The λ / 4 plate preferably has a layer containing a liquid crystal compound. When the λ / 4 plate has a layer containing a liquid crystal compound, the layer containing a liquid crystal compound may be a layer in which a liquid crystal compound horizontally aligned in one direction is fixed, or a layer in which a liquid crystal compound twisted in the thickness direction is fixed. The λ / 4 plate may also be a so-called broadband λ / 4 plate formed by laminating a layer that generates a λ / 4 retardation and a layer that generates a λ / 2 retardation. It is particularly preferred that at least one of the first λ / 4 plate 212 and the second λ / 4 plate 214 be a laminate consisting of a liquid crystal layer A in which a liquid crystal compound twisted in the thickness direction is fixed, and a liquid crystal layer B in which a liquid crystal compound twisted in the thickness direction is fixed. It is even more preferred that the first λ / 4 plate 212 and the second λ / 4 plate 214 be a laminate consisting of the liquid crystal layer A and the liquid crystal layer B. Furthermore, when the first λ / 4 plate 212 is a laminate made of the liquid crystal layer A and the liquid crystal layer B, it is preferable that the alignment direction of the liquid crystal compound on the surface of the first λ / 4 plate 212 facing the first liquid crystal layer 220 be parallel to the alignment direction of the liquid crystal compound on the surface of the first liquid crystal layer 220 facing the first λ / 4 plate 212. Furthermore, when the second λ / 4 plate 214 is a laminate made of the liquid crystal layer A and the liquid crystal layer B, it is preferable that the alignment direction of the liquid crystal compound 18 on the surface of the second λ / 4 plate 214 facing the second liquid crystal layer 224 be parallel to the alignment direction of the liquid crystal compound on the surface of the second liquid crystal layer 224 facing the second λ / 4 plate 214. Preferred embodiments (first and second embodiments) of the λ / 4 plate will be described below.

[0077] (First Aspect) A first aspect of the λ / 4 plate preferably used in the optical element of the present invention is a laminate consisting of a liquid crystal layer A in which a liquid crystal compound twisted in the thickness direction is fixed, and a liquid crystal layer B in which a liquid crystal compound twisted in the thickness direction is fixed. Here, in the first aspect, the twist direction of the liquid crystal compound in the liquid crystal layer A is the same as the twist direction of the liquid crystal compound in the liquid crystal layer B, the twist angle of the liquid crystal compound in the liquid crystal layer A is 26.5±10.0°, and the twist angle of the liquid crystal compound in the liquid crystal layer B is 78.6±10.0°. In addition, the in-plane slow axis of the surface of the liquid crystal layer A facing the liquid crystal layer B is parallel to the in-plane slow axis of the surface of the liquid crystal layer B facing the liquid crystal layer A. Furthermore, the refractive index anisotropy Δn of the liquid crystal layer A measured at a wavelength of 550 nm is A and the thickness d of the liquid crystal layer A A The product Δn A ・d A and the refractive index anisotropy Δn of the liquid crystal layer B measured at a wavelength of 550 nm. B and the thickness d of the liquid crystal layer B B The product Δn B ・d B and the values ​​thereof satisfy the following formula (A1) and formula (B1), respectively. A ・d A ≦312nm Formula (B1) 110nm≦Δn B ・d B ≦170 nm

[0078] The twist angle of the liquid crystal compound in liquid crystal layer A is preferably 26.5±8.0°, more preferably 26.5±6.0°. The twist angle of the liquid crystal compound in liquid crystal layer B is preferably 78.6±8.0°, more preferably 78.6±6.0°. The twist angle can be measured using an Axoscan (polarimeter) device manufactured by Axometrics and analysis software from the same company.

[0079] In addition, the above Δn A ・d A The value of Δn B ・d B It is preferable that the value of 262 nm≦Δn satisfies the following formula (A2) and formula (B2): A ・d A ≦302nm Formula (B2) 120nm≦ΔnB ・d B ≦160 nm Δn A ・d A The value of Δn B ・d B Similar to the method for measuring the twist angle, the angle can be measured using an Axoscan (polarimeter) device manufactured by Axometrics and analysis software from the same company.

[0080] Furthermore, the above Δn A ・d A The value of Δn B ・d B It is more preferable that the value of 272 nm≦Δn satisfies the following formula (A3) and formula (B3): A ・d A ≦292 nm Formula (B3) 130 nm≦Δn B ・d B ≦150 nm

[0081] An alignment film capable of regulating the alignment direction of the liquid crystal compound may be disposed between the liquid crystal layer A and the liquid crystal layer B, but it is preferable that no alignment film is disposed between the liquid crystal layer A and the liquid crystal layer B in order to obtain better adhesion between the liquid crystal layer A and the liquid crystal layer.

[0082] There are no particular limitations on the type of liquid crystal compound used to form the liquid crystal layer A and the liquid crystal layer B. As the liquid crystal layer A and the liquid crystal layer B, for example, a liquid crystal layer obtained by forming a low-molecular-weight liquid crystal compound in a nematic alignment in a liquid crystal state and then fixing the alignment by photocrosslinking or thermal crosslinking, or a liquid crystal layer obtained by forming a high-molecular-weight liquid crystal compound in a nematic alignment in a liquid crystal state and then fixing the alignment by cooling, can be used.

[0083] Generally, liquid crystal compounds can be classified into rod-shaped (rod-shaped liquid crystal compounds) and discotic (discotic liquid crystal compounds) types based on their shape. Each type is further divided into low-molecular-weight and high-molecular-weight types. High-molecular-weight compounds generally refer to compounds with a degree of polymerization of 100 or more (see "Polymer Physics / Phase Transition Dynamics," by Masao Doi, p. 2, Iwanami Shoten, 1992). While any liquid crystal compound can be used in the present invention, it is preferable to use rod-shaped or discotic liquid crystal compounds. A mixture of two or more rod-shaped liquid crystal compounds, two or more discotic liquid crystal compounds, or a mixture of a rod-shaped liquid crystal compound and a discotic liquid crystal compound may also be used. Preferably, the rod-shaped liquid crystal compound may be, for example, those described in claim 1 of JP-A-11-513019 or paragraphs

[0026] to

[0098] of JP-A-2005-289980. Preferably, the discotic liquid crystal compound may be, for example, those described in paragraphs

[0020] to

[0067] of JP-A-2007-108732 or paragraphs

[0013] to

[0108] of JP-A-2010-244038, but is not limited thereto. Liquid crystal layer A or liquid crystal layer B is preferably formed using a rod-shaped liquid crystal compound or discotic liquid crystal compound having a polymerizable group, as this can reduce temperature and humidity changes. The liquid crystal compound may be a mixture of two or more types, and in this case, it is preferable that at least one of the liquid crystal compounds has two or more polymerizable groups. In other words, the liquid crystal layer A or the liquid crystal layer B is preferably a layer formed by fixing a rod-shaped liquid crystal compound or a discotic liquid crystal compound having a polymerizable group by polymerization or the like, and in this case, after being formed into a layer, it is no longer necessary for the compound to exhibit liquid crystallinity. The type of polymerizable group contained in the discotic liquid crystal compound or the rod-shaped liquid crystal compound is not particularly limited, and a functional group capable of undergoing an addition polymerization reaction is preferred, and a polymerizable ethylenically unsaturated group or a ring-polymerizable group is preferred. More specifically, a (meth)acryloyl group, a vinyl group, a styryl group, an allyl group, etc. are preferred, and a (meth)acryloyl group is more preferred.

[0084] A λ / 4 plate can be produced by various methods. An example is as follows. First, a support such as a polymer film or a glass plate is prepared. An alignment film is formed thereon, if necessary. A liquid crystal layer A-forming composition containing a liquid crystal compound having a polymerizable group and, optionally, an additive such as a chiral agent is applied to the support surface or the alignment film surface to form a coating film. If desired, the coating film is heated to twist the molecules of the liquid crystal compound in the coating film into a twisted alignment. The coating film is then cooled to a solidification temperature, and polymerization is promoted by a curing treatment (ultraviolet irradiation (light irradiation treatment) or heat treatment) to fix the twisted alignment, thereby obtaining a liquid crystal layer A having optical rotation properties. The liquid crystal composition can be applied by a known method (e.g., wire bar coating, extrusion coating, direct gravure coating, reverse gravure coating, or die coating) using a coating solution of the liquid crystal composition containing the solvent described below. Alternatively, the liquid crystal layer A may be formed by discharging the coating liquid using an inkjet device. Next, a liquid crystal layer B-forming composition containing a liquid crystal compound having a polymerizable group and, if desired, an additive such as a chiral agent is applied onto the liquid crystal layer A (or onto the surface of an alignment film formed thereon as necessary) to form a coating film. The aligned liquid crystal compound having a polymerizable group is then subjected to a curing treatment (heating treatment or light irradiation treatment) to form a liquid crystal layer B. The liquid crystal layer A may be formed by directly applying the composition onto the liquid crystal polarization interference element 216 shown in FIG. 1 . Alternatively, the liquid crystal layer B may be applied directly onto the liquid crystal polarization interference element 216, and the liquid crystal layer A may be formed on the surface of the liquid crystal layer B opposite the liquid crystal polarization interference element 216 side. When the liquid crystal layer A is formed by applying the composition directly onto the liquid crystal polarization interference element 216 in this way, the alignment direction of the liquid crystal compound on the surface of the liquid crystal polarization interference element 216 facing the liquid crystal layer A tends to be parallel to the alignment direction of the liquid crystal compound on the surface of the liquid crystal polarization interference element 216 facing the liquid crystal polarization interference element 216. Furthermore, when liquid crystal layer B is formed by directly applying it onto the liquid crystal polarization interference element 216, the orientation direction of the liquid crystal compound on the surface of the liquid crystal polarization interference element 216 facing the liquid crystal layer B tends to be parallel to the orientation direction of the liquid crystal compound on the surface of the liquid crystal layer B facing the liquid crystal polarization interference element 216.

[0085] The aligned (preferably vertically aligned) liquid crystal compound is preferably fixed while maintaining the aligned state. Fixation is preferably carried out by a polymerization reaction of the polymerizable group introduced into the liquid crystal compound using a polymerization initiator. Polymerization reactions include thermal polymerization reactions using a thermal polymerization initiator and photopolymerization reactions using a photopolymerization initiator. Photopolymerization reactions are preferred. The amount of polymerization initiator used is preferably 0.01 to 20% by mass, more preferably 0.5 to 5% by mass, of the solid content of the composition.

[0086] When forming the liquid crystal layer A and the liquid crystal layer B, a chiral agent may be optionally used together with the liquid crystal compound. The chiral agent is added to impart a twisted alignment to the liquid crystal compound. However, of course, if the liquid crystal compound is an optically active compound, such as one having an asymmetric carbon atom in the molecule, the addition of a chiral agent is not necessary. Furthermore, depending on the manufacturing method and twist angle, the addition of a chiral agent may not be necessary. There are no particular limitations on the structure of the chiral agent, as long as it is compatible with the liquid crystal compound used in combination. Any known chiral agent (e.g., described in "Liquid Crystal Device Handbook," edited by the Japan Society for the Promotion of Science, Committee 142, Chapter 3, Section 4-3, "Chiral Agents for TN and STN," p. 199, 1989) can be used. Chiral agents generally contain an asymmetric carbon atom, but axially asymmetric or planarly asymmetric compounds without an asymmetric carbon atom can also be used as chiral agents. Examples of axially asymmetric or planarly asymmetric compounds include binaphthyl, helicene, paracyclophane, and their derivatives. The chiral agent may also have liquid crystal properties.

[0087] The uniformity of the coating film, film strength, alignment of the liquid crystal compound, etc. can be improved by using a plasticizer, a surfactant, a polymerizable monomer, etc. together with the liquid crystal compound. It is preferable that these materials are compatible with the liquid crystal compound and do not inhibit alignment. Furthermore, an additive (alignment control agent) that promotes horizontal alignment or vertical alignment may be used to make the liquid crystal compound horizontally or vertically aligned. Various known additives can be used.

[0088] The polymerizable monomer may be a radically polymerizable or cationic polymerizable compound. A polyfunctional radically polymerizable monomer is preferred, and one that is copolymerizable with the above-mentioned polymerizable group-containing liquid crystal compound is preferable. For example, the monomers described in paragraphs

[0018] to

[0020] of JP-A No. 2002-296423 are exemplified. The amount of the compound added is generally in the range of 1 to 50% by mass, preferably 5 to 30% by mass, based on the liquid crystal molecules.

[0089] Examples of surfactants include conventionally known compounds, and fluorine-based compounds are particularly preferred. Specific examples include the compounds described in paragraphs

[0028] to

[0056] of JP-A No. 2001-330725 and the compounds described in paragraphs

[0069] to

[0126] of JP-A No. 2003-295212.

[0090] The polymer used together with the liquid crystal compound is preferably capable of thickening the coating solution. An example of the polymer is cellulose ester. Preferred examples of cellulose ester include those described in paragraph

[0178] of JP-A No. 2000-155216. In order not to inhibit the alignment of the liquid crystal compound, the amount of the polymer added is preferably in the range of 0.1 to 10% by mass, more preferably 0.1 to 8% by mass, relative to the liquid crystal molecules. The discotic nematic liquid crystal phase-solid phase transition temperature of the liquid crystal compound is preferably 70 to 300°C, more preferably 70 to 170°C.

[0091] As the solvent used in preparing the composition (coating liquid), an organic solvent is preferably used. Examples of the organic solvent include amides (e.g., N,N-dimethylformamide), sulfoxides (e.g., dimethyl sulfoxide), heterocyclic compounds (e.g., pyridine), hydrocarbons (e.g., benzene, hexane), alkyl halides (e.g., chloroform, dichloromethane), esters (e.g., methyl acetate, ethyl acetate, butyl acetate), ketones (e.g., acetone, methyl ethyl ketone), and ethers (e.g., tetrahydrofuran, 1,2-dimethoxyethane). Alkyl halides and ketones are preferred. Two or more organic solvents may be used in combination.

[0092] In the first embodiment, the liquid crystal layer A-forming composition or the liquid crystal layer B-forming composition may be applied to the surface of the alignment film to align the molecules of a liquid crystal compound (e.g., a discotic liquid crystal compound). The alignment film can be formed by means of rubbing an organic compound (preferably a polymer), oblique deposition of an inorganic compound, formation of a layer having microgrooves, or deposition of an organic compound (e.g., ω-tricosanoic acid, dioctadecylmethylammonium chloride, methyl stearate) by the Langmuir-Blodgett method (LB film). Furthermore, alignment films that exhibit alignment function upon application of an electric field, a magnetic field, or light irradiation (preferably polarized light) are also known. The alignment film is preferably formed by rubbing a polymer.

[0093] Examples of the polymer include methacrylate copolymers, styrene copolymers, polyolefins, polyvinyl alcohol and modified polyvinyl alcohol, poly(N-methylolacrylamide), polyesters, polyimides, vinyl acetate copolymers, carboxymethyl cellulose, polycarbonates, etc., as described in paragraph

[0022] of JP-A-8-338913. A silane coupling agent can be used as the polymer. Water-soluble polymers (e.g., poly(N-methylolacrylamide), carboxymethyl cellulose, gelatin, polyvinyl alcohol, and modified polyvinyl alcohol) are preferred, with gelatin, polyvinyl alcohol, and modified polyvinyl alcohol being more preferred, and polyvinyl alcohol and modified polyvinyl alcohol being most preferred.

[0094] The alignment film can be basically formed by applying a solution containing the above-mentioned polymer, which is the alignment film-forming material, and optional additives (e.g., a crosslinking agent) to a transparent support, followed by heating and drying (crosslinking), followed by rubbing. The rubbing treatment can be a treatment method widely used as a liquid crystal alignment treatment process for LCDs. That is, a method can be used in which the surface of the alignment film is rubbed in a certain direction with paper, gauze, felt, rubber, nylon, polyester fiber, or the like to obtain alignment. Generally, rubbing is performed several times using a cloth with fibers of uniform length and thickness evenly flocked.

[0095] When the first embodiment of the λ / 4 plate preferably used in the optical element of the present invention is used, the liquid crystal layer A is preferably disposed on the optical laminate side.

[0096] (Second Aspect) A second aspect of the λ / 4 plate preferably used in the optical element of the present invention is a laminate consisting of a liquid crystal layer A in which a liquid crystal compound twisted in the thickness direction is fixed, and a liquid crystal layer B in which a liquid crystal compound twisted in the thickness direction is fixed. Here, in the second aspect, the twist direction of the liquid crystal compound in the liquid crystal layer A is the same as the twist direction of the liquid crystal compound in the liquid crystal layer B, the twist angle of the liquid crystal compound in the liquid crystal layer A is 59.7±10.0°, and the twist angle of the liquid crystal compound in the liquid crystal layer B is 127.6±10.0°. In addition, the in-plane slow axis of the surface of the liquid crystal layer A facing the liquid crystal layer B is parallel to the in-plane slow axis of the surface of the liquid crystal layer B facing the liquid crystal layer A. Furthermore, the refractive index anisotropy Δn of the liquid crystal layer A measured at a wavelength of 550 nm is A and the thickness d of the liquid crystal layer A A The product Δn A ・d A and the refractive index anisotropy Δn of the liquid crystal layer B measured at a wavelength of 550 nm. B and the thickness d of the liquid crystal layer B B The product Δn B ・d B and the values ​​thereof satisfy the following formula (A4) and formula (B4), respectively. A ・d A ≦171nm Formula (B4) 252nm≦Δn B ・d B≦312 nm

[0097] The twist angle of the liquid crystal compound in liquid crystal layer A is preferably 59.7±8.0°, more preferably 59.7±6.0°. The twist angle of the liquid crystal compound in liquid crystal layer B is preferably 127.6±8.0°, more preferably 127.6±6.0°. The twist angle can be measured using an Axoscan (polarimeter) device manufactured by Axometrics and analysis software from the same company.

[0098] In addition, the above Δn A ・d A The value of Δn B ・d B It is preferable that the value of Δn satisfies the following formula (A5) and formula (B5): Formula (A5) 121 nm≦Δn A ・d A ≦161nm Formula (B5) 262nm≦Δn B ・d B ≦302 nm Δn A ・d A The value of Δn B ・d B Similar to the method for measuring the twist angle, the angle can be measured using an Axoscan (polarimeter) device manufactured by Axometrics and analysis software from the same company.

[0099] Furthermore, the above Δn A ・d A The value of Δn B ・d B It is more preferable that the value of Δn satisfies the following formula (A6) and formula (B6): 131 nm≦Δn A ・d A ≦151nm Formula (B6) 272nm≦Δn B ・d B ≦292 nm

[0100] An alignment film capable of regulating the alignment direction of the liquid crystal compound may be disposed between the liquid crystal layer A and the liquid crystal layer B, but it is preferable that no alignment film is disposed between the liquid crystal layer A and the liquid crystal layer B in order to obtain better adhesion between the liquid crystal layer A and the liquid crystal layer.

[0101] The materials constituting the liquid crystal layer A and the liquid crystal layer B are exemplified by the above-described materials constituting the liquid crystal layer A and the liquid crystal layer B. The method for manufacturing the liquid crystal layer A and the liquid crystal layer B is not particularly limited, and the above-described methods for manufacturing the liquid crystal layer A and the liquid crystal layer B are exemplified.

[0102] When the second embodiment of the λ / 4 plate preferably used in the optical element of the present invention is used, the liquid crystal layer A is preferably disposed on the optical laminate side.

[0103] <Optical Element> The optical element of the present invention includes a plurality of optically anisotropic layers formed using a composition containing a liquid crystal compound, each having a liquid crystal orientation pattern in which the orientation of the optical axis derived from the liquid crystal compound changes while continuously rotating along at least one in-plane direction, and the optical element of the present invention is disposed between at least one pair of adjacent optically anisotropic layers in the plurality of optically anisotropic layers. Herein, in the liquid crystal orientation pattern of the optically anisotropic layers, when the length of a 180° rotation of the orientation of the optical axis derived from the liquid crystal compound in one direction in which the orientation of the optical axis derived from the liquid crystal compound changes while continuously rotating is defined as one period, at least one optically anisotropic layer has a different length of one period from the other optically anisotropic layers. As described above, the optical element of the present invention acts as a wavelength-selective retardation plate for circularly polarized light. Hereinafter, the optical element of the present invention may be referred to as a "wavelength-selective retardation plate."

[0104] The optical element of the present invention has a small wavelength dependency of the refraction angle of incident and transmitted light, and can emit light of different wavelengths incident from the same direction in almost the same direction.

[0105] An example of the optical element of the present invention is shown in Figure 6. The optical element 10 shown in Figure 6 includes a first optically anisotropic member 12, a second optically anisotropic member 14, and a wavelength-selective retardation plate 18G disposed between the first optically anisotropic member 12 and the second optically anisotropic member 14. As described above, the optical element of the present invention includes an optically anisotropic layer formed using a composition containing a liquid crystal compound and having a predetermined liquid crystal orientation pattern in which the optical axis derived from the liquid crystal compound rotates, arranged in the thickness direction. The first optically anisotropic member 12 includes a support 20, an alignment film 24A, and a first optically anisotropic layer 26A. The second optically anisotropic member 14 includes a support 20, an alignment film 24B, and a second optically anisotropic layer 26B. In the optical element of the present invention, as described above, the wavelength-selective retardation plate converts circularly polarized light in a specific wavelength range (first wavelength range) into circularly polarized light in the opposite rotation direction, and transmits (passes through) light in the other second wavelength range as is. In the illustrated optical element 10, the wavelength-selective retardation plate 18G converts the rotation direction of the circularly polarized light of the green light into the opposite rotation direction, and transmits the other light as circularly polarized light of the same rotation direction.

[0106] Although not shown in the figures, the first optically anisotropic member 12 and the wavelength-selective retardation plate 18G, and the wavelength-selective retardation plate 18G and the second optically anisotropic member 14 are bonded together by bonding layers provided between the layers. The optical element of the present invention may be configured by stacking the first optically anisotropic member 12, the wavelength-selective retardation plate 18G, and the second optically anisotropic member 14 and holding them with a frame, a jig, or the like. The optical element of the present invention is not limited to the configuration in which the first optically anisotropic member 12, the wavelength-selective retardation plate 18G, and the second optically anisotropic member 14 are stacked in close contact as in the illustrated example, and a configuration in which one or more of these members are arranged at a distance from each other may also be used.

[0107] Furthermore, although the illustrated optical element 10 has a support 20 for each optically anisotropic member, the optical element of the present invention does not necessarily need to have a support 20 for each optically anisotropic member. For example, the optical element of the present invention may have a configuration in which a wavelength-selective retardation plate 18G is formed on the surface of the second optically anisotropic member 14 (second optically anisotropic layer 26B), an alignment film 24A is formed thereon, and a first optically anisotropic layer 26A is formed thereon. Alternatively, the optical element of the present invention may be configured from the above configuration by peeling off the support 20 of the second optically anisotropic member 14, leaving only the wavelength-selective retardation plate, alignment film, and optically anisotropic layer, or by peeling off the alignment film as well, leaving only the wavelength-selective retardation plate and optically anisotropic layer.

[0108] That is, the optical element of the present invention has an arrangement of a plurality of optically anisotropic layers, a wavelength-selective retardation plate between at least one pair of adjacent optically anisotropic layers, and the optically anisotropic layers have a liquid crystal orientation pattern in which the direction of the optical axis derived from the liquid crystal compound rotates in one direction, and further, various layer configurations can be used as long as the liquid crystal orientation pattern of at least one optically anisotropic layer has a different period as described below.

[0109] [Optical Anisotropic Member] The optical element 10 of the present invention includes a wavelength-selective retardation plate 18G provided between a first optical anisotropic member 12 and a second optical anisotropic member 14. As described above, the first optical anisotropic member 12 includes a support 20, an alignment film 24A, and a first optical anisotropic layer 26A. The second optical anisotropic member 14 includes a support 20, an alignment film 24B, and a second optical anisotropic layer 26B.

[0110] (Support) In the first optically anisotropic member 12 and the second optically anisotropic member 14, the support 20 supports the alignment films 24A and 24B, as well as the first optically anisotropic layer 26A and the second optically anisotropic layer 26B. In the following description, when it is not necessary to distinguish between the alignment films 24A and 24B, the alignment films 24A and 24B will also be collectively referred to as "alignment films." Furthermore, in the following description, when it is not necessary to distinguish between the first optically anisotropic layer 26A and the second optically anisotropic layer 26B, the first optically anisotropic layer 26A and the second optically anisotropic layer 26B will also be collectively referred to as "optically anisotropic layers."

[0111] The support 20 may be any sheet-like material (film, plate-like material) that can support the alignment film and the optically anisotropic layer.

[0112] (Alignment film) In the first optically anisotropic member 12, an alignment film 24A is formed on the surface of the support 20. In the second optically anisotropic member 14, an alignment film 24B is formed on the surface of the support 20. The alignment film 24A is an alignment film for orienting the liquid crystal compound 30 in a predetermined liquid crystal alignment pattern when forming the first optically anisotropic layer 26A of the first optically anisotropic member 12. The alignment film 24B is an alignment film for orienting the liquid crystal compound 30 in a predetermined liquid crystal alignment pattern when forming the second optically anisotropic layer 26B of the second optically anisotropic member 14.

[0113] As will be described later, in the optical element 10 of the present invention, the optically anisotropic layer has a liquid crystal orientation pattern in which the orientation of the optical axis 30A (see FIG. 6 ) derived from the liquid crystal compound 30 changes while continuously rotating along one in-plane direction (the direction of the arrow X described later). Therefore, the orientation film of each optically anisotropic member is formed so that the optically anisotropic layer can form this liquid crystal orientation pattern. In the optical element of the present invention, when the length of a 180° rotation of the orientation of the optical axis 30A in one direction in which the orientation of the optical axis 30A changes while continuously rotating in the liquid crystal orientation pattern is defined as one period (optical axis rotation period), at least one optically anisotropic layer has a liquid crystal orientation pattern whose length differs from that of the other optically anisotropic layers. In the optical element 10 shown in FIG. 6 , one period (one period Λ) of the liquid crystal orientation pattern in the first optically anisotropic layer 26A is A ) is one period (one period Λ) of the liquid crystal alignment pattern in the second optically anisotropic layer 26B. B ) is shorter than

[0114] In the following description, "the orientation of the optical axis 30A rotates" may also be simply referred to as "the optical axis 30A rotates."

[0115] Various known alignment films can be used, including, for example, a rubbed film made of an organic compound such as a polymer, an obliquely evaporated film of an inorganic compound, a film having microgrooves, and a film formed by accumulating LB (Langmuir-Blodgett) films made of organic compounds such as ω-tricosanoic acid, dioctadecylmethylammonium chloride, and methyl stearate by the Langmuir-Blodgett method.

[0116] An alignment film formed by rubbing treatment can be formed by rubbing the surface of the polymer layer several times in a certain direction with paper or cloth. Preferred examples of materials used for the alignment film include polyimide, polyvinyl alcohol, polymers having polymerizable groups described in JP-A-9-152509, and materials used to form alignment films described in JP-A-2005-97377, JP-A-2005-99228, and JP-A-2005-128503.

[0117] In the optical element 10 of the present invention, the alignment film is preferably a so-called photo-alignment film obtained by irradiating a photo-alignable material with polarized or non-polarized light. That is, in the optical element 10 of the present invention, the alignment film is preferably a photo-alignment film formed by applying a photo-alignment material onto the support 20. Irradiation with polarized light can be performed on the photo-alignment film from a vertical direction or an oblique direction, and irradiation with non-polarized light can be performed on the photo-alignment film from an oblique direction.

[0118] Examples of photo-alignment materials that can be used in the photo-alignment film of the present invention include those disclosed in JP-A Nos. 2006-285197, 2007-76839, 2007-138138, 2007-94071, 2007-121721, 2007-140465, 2007-156439, and JP-A Nos. azo compounds described in JP-A-2007-133184, JP-A-2009-109831, Japanese Patent Nos. 3,883,848 and 4,151,746; aromatic ester compounds described in JP-A-2002-229039; maleic anhydrides having photo-orientable units described in JP-A-2002-265541 and JP-A-2002-317013; Preferred examples include imide and / or alkenyl-substituted nadimide compounds, photocrosslinkable silane derivatives described in Japanese Patent Nos. 4205195 and 4205198, photocrosslinkable polyimides, photocrosslinkable polyamides and photocrosslinkable esters described in JP-T-2003-520878, JP-T-2004-529220 and JP-T-4162850, and photodimerizable compounds described in JP-A-9-118717, JP-A-10-506420, JP-A-2003-505561, WO 2010 / 150748, JP-A-2013-177561 and JP-A-2014-12823, particularly cinnamate compounds, chalcone compounds and coumarin compounds. Among these, azo compounds, photocrosslinkable polyimides, photocrosslinkable polyamides, photocrosslinkable esters, cinnamate compounds, and chalcone compounds are preferably used.

[0119] There is no limitation on the thickness of the alignment film, and it may be set appropriately depending on the material of which the alignment film is formed so as to obtain the necessary alignment function. The thickness of the alignment film is preferably 0.01 to 5 μm, and more preferably 0.05 to 2 μm.

[0120] There is no limitation on the method for forming the alignment film, and various known methods can be used depending on the material for forming the alignment film. One example is a method in which an alignment film is applied to the surface of the support 20, dried, and then exposed to laser light to form an alignment pattern.

[0121] An example of an exposure device for forming an alignment pattern by exposing an alignment film is conceptually shown in Fig. 17. Note that, although the example shown in Fig. 17 illustrates exposure of the alignment film 24A of the first optical anisotropic member 12, an alignment pattern can also be formed on the alignment film 24B of the second optical anisotropic member 14 in the same manner using the same exposure device.

[0122] The exposure device 60 shown in Figure 17 includes a light source 64 equipped with a laser 62, a λ / 2 plate (not shown) that changes the polarization direction of laser light M emitted by the laser 62, a beam splitter 68 that splits the laser light M emitted by the laser 62 and passed through the λ / 2 plate (not shown) into two beams MA and MB, mirrors 70A and 70B that are respectively arranged on the optical paths of the two split beams MA and MB, and λ / 4 plates 72A and 72B. Although not shown, the light source 64 includes a polarizing plate and emits linearly polarized light P0. The λ / 4 plates 72A and 72B have optical axes that are orthogonal to each other. The λ / 4 plate 72A splits the linearly polarized light P0 0 (ray MA) is polarized by right-handed circular polarization P R The λ / 4 plate 72B is a linearly polarized light P 0 (Light ray MB) is polarized by left-handed circular polarization P L are converted to , respectively.

[0123] The support 20 having the alignment film 24A before the alignment pattern is formed is placed in an exposure unit, and two light beams MA and MB are caused to intersect and interfere on the alignment film 24A, and the alignment film 24A is irradiated with the interference light to expose it. This interference causes the polarization state of the light irradiated on the alignment film 24A to periodically change in the form of interference fringes. This results in an alignment pattern in which the alignment state periodically changes on the alignment film 24A. In the exposure device 60, the period of the alignment pattern can be adjusted by changing the crossing angle α of the two light beams MA and MB. That is, in the exposure device 60, by adjusting the crossing angle α, the length of one period (one period Λ) in which the optical axis 30A originating from the liquid crystal compound 30 rotates 180° in one direction of the rotation of the optical axis 30A can be adjusted. By forming an optically anisotropic layer on an alignment film having such an alignment pattern in which the alignment state changes periodically, it is possible to form a first optically anisotropic layer 26A having a liquid crystal alignment pattern in which the optic axis 30A derived from the liquid crystal compound 30 continuously rotates in one direction, as will be described later. In addition, by rotating the optic axes of the λ / 4 plates 72A and 72B by 90° each, the rotation direction of the optic axis 30A can be reversed.

[0124] In the optical element of the present invention, the alignment film is provided as a preferred embodiment but is not an essential component. For example, by forming an alignment pattern on the support 20 by a method of rubbing the support 20 or a method of processing the support 20 with laser light or the like, it is possible to configure the first optically anisotropic layer 26A etc. to have a liquid crystal alignment pattern in which the direction of the optic axis 30A derived from the liquid crystal compound 30 changes while continuously rotating along at least one direction in the plane.

[0125] <<Optical Anisotropic Layer>> In the first optically anisotropic member 12, a first optically anisotropic layer 26A is formed on the surface of the alignment film 24A. In the second optically anisotropic member 14, a second optically anisotropic layer 26B is formed on the surface of the alignment film 24B. Note that in FIG. 6 (and FIGS. 9 to 11 described below), in order to simplify the drawings and clearly show the configuration of the optical element 10, both the first optically anisotropic layer 26A and the second optically anisotropic layer 26B only show the liquid crystal compound 30 (liquid crystal compound molecules) on the surface of the alignment film. However, as conceptually shown in FIG. 7 exemplarily illustrating the first optically anisotropic layer 26A, the first optically anisotropic layer 26A and the second optically anisotropic layer 26B have a structure in which aligned liquid crystal compounds 30 are stacked, similar to an optically anisotropic layer formed using a composition containing a normal liquid crystal compound.

[0126] As described above, in the optical element 10 of the present invention, the optically anisotropic layers (first optically anisotropic layer 26A and second optically anisotropic layer 26B) are formed using a composition containing a liquid crystal compound. When the in-plane retardation value of the optically anisotropic layer is set to λ / 2, the optically anisotropic layer functions as a general λ / 2 plate, that is, imparts a phase difference of half the wavelength, i.e., 180°, to two orthogonal linearly polarized components contained in light incident on the optically anisotropic layer.

[0127] The optically anisotropic layer has a liquid crystal orientation pattern in which the direction of the optical axis derived from the liquid crystal compound changes while continuously rotating in one direction indicated by arrow X within the plane of the optically anisotropic layer. The optical axis 30A derived from the liquid crystal compound 30 is the axis along which the refractive index of the liquid crystal compound 30 is highest, i.e., the slow axis. For example, when the liquid crystal compound 30 is a rod-shaped liquid crystal compound, the optical axis 30A is aligned along the long axis direction of the rod shape. In the following description, the "one direction indicated by arrow X" will also be referred to simply as the "arrow X direction." In the following description, the optical axis 30A derived from the liquid crystal compound 30 will also be referred to as the "optical axis 30A of the liquid crystal compound 30" or "optical axis 30A." In the optically anisotropic layer, the liquid crystal compound 30 is two-dimensionally aligned in a plane parallel to the arrow X direction and the Y direction perpendicular to the arrow X direction. In FIGS. 6 and 7, and FIGS. 9 to 11, which will be described later, the Y direction is perpendicular to the paper surface.

[0128] FIG. 8 conceptually shows a plan view of the first optically anisotropic layer 26A. The plan view is a view of the optical element 10 in FIG. 6 as seen from above, i.e., a view of the optical element 10 as seen in the thickness direction (i.e., the stacking direction of the layers (films)). In other words, a view of the first optically anisotropic layer 26A as seen in a direction perpendicular to the main surface. Furthermore, in FIG. 8, in order to clearly show the configuration of the optical element 10 of the present invention, only the liquid crystal compound 30 on the surface of the alignment film 24A is shown, as in FIG. 3. However, as described above, the first optically anisotropic layer 26A has a structure in which the liquid crystal compound 30 is stacked in the thickness direction, starting from the liquid crystal compound 30 on the surface of the alignment film 24A, as shown in FIG. 7.

[0129] 8, the first optically anisotropic layer 26A will be described as a representative example, but the second optically anisotropic layer 26B basically has the same configuration and functions and effects, except for the length of one period (one period Λ) of the liquid crystal alignment pattern, which will be described later. The rotation directions of the optical axis 30A are opposite between the first optically anisotropic layer 26A and the second optically anisotropic layer 26B. That is, when the rotation of the optical axis 30A in the first optically anisotropic layer 26A is clockwise, the rotation of the optical axis 30A in the second optically anisotropic layer is counterclockwise.

[0130] The first optically anisotropic layer 26A has a liquid crystal alignment pattern in which the orientation of the optical axis 30A derived from the liquid crystal compound 30 changes while continuously rotating along the direction of arrow X within the plane of the first optically anisotropic layer 26A. The phrase "the orientation of the optical axis 30A of the liquid crystal compound 30 changes while continuously rotating in the direction of arrow X (a predetermined direction)" specifically means that the angle formed between the optical axis 30A of the liquid crystal compound 30 aligned along the direction of arrow X and the direction of arrow X varies depending on the position in the direction of arrow X, and the angle formed between the optical axis 30A and the direction of arrow X sequentially changes along the direction of arrow X from θ to θ+180° or θ−180°. The difference in angle between the optical axes 30A of the liquid crystal compounds 30 adjacent to each other in the direction of arrow X is preferably 45° or less, more preferably 15° or less, and even more preferably a smaller angle.

[0131] On the other hand, the liquid crystal compounds 30 forming the first optically anisotropic layer 26A are arranged at equal intervals in the Y direction perpendicular to the direction of the arrow X, i.e., in the Y direction perpendicular to the direction in which the optical axes 30A continuously rotate. In other words, among the liquid crystal compounds 30 forming the first optically anisotropic layer 26A, the liquid crystal compounds 30 aligned in the Y direction have the same angle between the direction of the optical axes 30A and the direction of the arrow X.

[0132] In the optical element 10 of the present invention, in the liquid crystal orientation pattern of the liquid crystal compound 30, the length (distance) over which the optical axis 30A of the liquid crystal compound 30 rotates 180° in the direction of arrow X, in which the orientation of the optical axis 30A continuously changes in plane, is defined as the length Λ of one period of the liquid crystal orientation pattern. In other words, the length of one period of the liquid crystal orientation pattern is defined as the distance from the angle θ between the optical axis 30A of the liquid crystal compound 30 and the direction of arrow X to the angle θ + 180°. That is, the length Λ of one period is defined as the distance between the centers of two liquid crystal compounds 30 in the direction of arrow X that have the same angle with respect to the direction of arrow X. Specifically, as shown in FIG. 8 , the length Λ of one period is defined as the distance between the centers of two liquid crystal compounds 30 in the direction of arrow X whose optical axes 30A coincide with the direction of arrow X. In the following description, this length Λ of one period is also referred to as "one period Λ." In the following description, in order to distinguish one period Λ in each optically anisotropic layer, one period Λ in the first optically anisotropic layer 26A will be referred to as "Λ A ", one period Λ in the second optically anisotropic layer 26B is "Λ B In the optical element 10 of the present invention, the liquid crystal alignment pattern of the optically anisotropic layer repeats this one period Λ in the direction of arrow X, that is, in one direction in which the direction of the optical axis 30A changes by continuously rotating.

[0133] As described above, in the optically anisotropic layer, the liquid crystal compounds aligned in the Y direction have the same angle between their optical axes 30A and the direction of arrow X (one direction in which the optical axes of the liquid crystal compounds 30 rotate). A region in which the liquid crystal compounds 30, with the same angle between their optical axes 30A and the direction of arrow X, are arranged in the Y direction, is referred to as region R. In this case, the in-plane retardation (Re) value in each region R is preferably half the wavelength, i.e., λ / 2. These in-plane retardations are calculated by the product of the refractive index difference Δn associated with the refractive index anisotropy of region R and the thickness of the optically anisotropic layer. Here, the refractive index difference associated with the refractive index anisotropy of region R in the optically anisotropic layer is a refractive index difference defined by the difference between the refractive index in the direction of the slow axis in the plane of region R and the refractive index in the direction perpendicular to the direction of the slow axis. That is, the refractive index difference Δn due to the refractive index anisotropy of region R is equal to the difference between the refractive index of liquid crystal compound 30 in the direction of optical axis 30A and the refractive index of liquid crystal compound 30 in the direction perpendicular to optical axis 30A in the plane of region R. In other words, the refractive index difference Δn is equal to the refractive index difference of the liquid crystal compound.

[0134] When circularly polarized light is incident on such optically anisotropic layers (first optically anisotropic layer 26A and second optically anisotropic layer 26B), the light is refracted and the direction of the circularly polarized light is converted. This action is conceptually shown in FIG. 9, exemplifying the first optically anisotropic layer 26A. It is assumed that the product of the refractive index difference of the liquid crystal compound and the thickness of the optically anisotropic layer in the first optically anisotropic layer 26A is λ / 2. As shown in FIG. 9, when the product of the refractive index difference of the liquid crystal compound in the first optically anisotropic layer 26A and the thickness of the optically anisotropic layer is λ / 2, left-handed circularly polarized incident light L 1 When incident, the incident light L 1 is given a phase difference of 180° by passing through the first optically anisotropic layer 26A, and becomes the transmitted light L 2 is converted to right-handed circularly polarized light.

[0135] On the other hand, as conceptually shown in FIG. 10, when the product of the refractive index difference of the liquid crystal compound of the first optically anisotropic layer 26A and the thickness of the optically anisotropic layer is λ / 2, right-handed circularly polarized incident light L 4 When incident, the incident light L 4is given a phase difference of 180° by passing through the first optically anisotropic layer 26A, and becomes the left-handed circularly polarized transmitted light L 5 is converted to

[0136] In the first optically anisotropic layer 26A, the in-plane retardation value of the plurality of regions R is preferably a half wavelength. The in-plane retardation Re(550) of the plurality of regions R of the first optically anisotropic layer 26A for incident light having a wavelength of 550 nm is expressed as Re(550)=Δn 550 ×d is preferably within the range defined by the following formula (1): 550 is the refractive index difference due to the refractive index anisotropy of the region R when the wavelength of incident light is 550 nm, and d is the thickness of the first optically anisotropic layer 26A. 550 ×d≦350 nm (1) That is, the in-plane retardation Re(550) of the plurality of regions R of the first optically anisotropic layer 26A=Δn 550 When ×d satisfies the formula (1), a sufficient amount of the circularly polarized component of the light incident on the first optically anisotropic layer 26A can be converted into circularly polarized light traveling in a direction inclined forward or backward with respect to the direction of the arrow X. In-plane retardation Re(550)=Δn 550 ×d is 225 nm≦Δn 550 ×d≦340 nm is more preferable, and 250 nm≦Δn 550 It is more preferable that ×d≦330 nm. The above formula (1) is a range for incident light having a wavelength of 550 nm, but the in-plane retardation Re(λ) of the plurality of regions R of the optically anisotropic layer for incident light having a wavelength of λ nm is λ ×d is preferably within the range defined by the following formula (1-2), and can be set appropriately: 0.7 λnm≦Δn λ ×d≦1.3λnm...(1-2)

[0137] Furthermore, the in-plane retardation values ​​of the regions R in the first optically anisotropic layer 26A may be outside the range of the above formula (1). 550 ×d<200 nm or 350 nm<Δn 550×d, it is possible to separate light into light traveling in the same direction as the incident light and light traveling in a direction different from the incident light. 550 When ×d approaches 0 nm or 550 nm, the component of light traveling in the same direction as the incident light increases, and the component of light traveling in a direction different from the incident light decreases.

[0138] Furthermore, the in-plane retardation Re(450) of each region R of the first optically anisotropic layer 26A for incident light having a wavelength of 450 nm is expressed as Re(450)=Δn 450 ×d and the in-plane retardation Re(550)=Δn of each region R of the first optically anisotropic layer 26A for incident light having a wavelength of 550 nm. 550 ×d preferably satisfies the following formula (2): 450 is the refractive index difference associated with the refractive index anisotropy of the region R when the wavelength of the incident light is 450 nm. (Δn 450 × d) / (Δn 550 ×d)<1.0 (2) Formula (2) indicates that the liquid crystal compound 30 contained in the first optically anisotropic layer 26A has reverse dispersion. That is, when formula (2) is satisfied, the first optically anisotropic layer 26A can accommodate incident light over a wide wavelength range.

[0139] Here, by changing one period Λ of the liquid crystal alignment pattern formed in the first optically anisotropic layer 26A, the transmitted light L 2 and L 5 Specifically, the shorter the period Λ of the liquid crystal alignment pattern, the stronger the interference between the lights passing through the adjacent liquid crystal compounds 30, and therefore the angle of refraction of the transmitted light L 2 and L 5 In addition, the incident light L 1 and L 4 Transmitted light L 2 and L 5 The angle of refraction of the incident light L 1 and L 4 (Transmitted light L 2 and L 5) . Specifically, the longer the wavelength of the incident light, the greater the refraction of the transmitted light. That is, when the incident light is red, green, and blue, the red light is refracted the most and the blue light is refracted the least. Furthermore, by reversing the rotation direction of the optical axis 30A of the liquid crystal compound 30, which rotates along the direction of arrow X, the refraction direction of the transmitted light can be reversed.

[0140] The optically anisotropic layer comprises a cured layer of a liquid crystal composition containing a rod-shaped or discotic liquid crystal compound, and has a liquid crystal alignment pattern in which the optical axis of the rod-shaped or discotic liquid crystal compound is aligned as described above. An alignment film is formed on a support 20, and a liquid crystal composition is applied to the alignment film and cured to obtain an optically anisotropic layer comprising a cured layer of the liquid crystal composition. While the optically anisotropic layer functions as a so-called λ / 2 plate, the present invention also includes an embodiment in which a laminate integrally comprising the support 20 and the alignment film functions as a λ / 2 plate. The liquid crystal composition for forming the optically anisotropic layer contains a rod-shaped or discotic liquid crystal compound, and may further contain other components such as a leveling agent, an alignment control agent, a polymerization initiator, and an alignment aid.

[0141] Furthermore, the optically anisotropic layer preferably has a broadband with respect to the wavelength of incident light, and is preferably constructed using a liquid crystal material whose birefringence exhibits reverse dispersion. It is also preferable to impart a twist component to the liquid crystal composition or to laminate different retardation layers, thereby making the optically anisotropic layer substantially broadband with respect to the wavelength of incident light. For example, JP 2014-089476 A discloses a method for realizing a broadband patterned λ / 2 plate by laminating two layers of liquid crystal with different twist directions in an optically anisotropic layer, and this method can be preferably used in the present invention.

[0142] Rod-shaped liquid crystal compounds include azomethines, azoxy compounds, cyanobiphenyls, cyanophenyl esters, benzoates, cyclohexanecarboxylic acid phenyl esters, cyanophenylcyclohexanes, cyano-substituted phenylpyrimidines, alkoxy-substituted phenylpyrimidines, phenyldioxanes, tolanes, and alkenylcyclohexylbenzonitriles. Not only low-molecular-weight liquid crystal molecules such as those mentioned above, but also polymeric liquid crystal molecules can be used.

[0143] It is more preferable to fix the alignment of the rod-shaped liquid crystal compound by polymerization. Examples of polymerizable rod-shaped liquid crystal compounds include those described in Makromol. Chem. , Vol. 190, p. 2255 (1989), Advanced Materials Vol. 5, p. 107 (1993), U.S. Patent Nos. 4,683,327, 5,622,648, 5,770,107, WO 95 / 22586, 95 / 24455, 97 / 00600, 98 / 23580, 98 / 52905, JP-A-1-272551, JP-A-6-16616, JP-A-7-110469, JP-A-11-80081, and compounds described in Japanese Patent Application No. 2001-64627 can be used. Furthermore, as the rod-shaped liquid crystal compound, for example, those described in JP-A-11-513019 and JP-A-2007-279688 can also be preferably used.

[0144] Discotic Liquid Crystal Compound: As the discotic liquid crystal compound, for example, those described in JP-A Nos. 2007-108732 and 2010-244038 can be preferably used. When a discotic liquid crystal compound is used in the optically anisotropic layer, the liquid crystal compound 30 stands up in the thickness direction in the optically anisotropic layer, and the optic axis 30A derived from the liquid crystal compound is defined as an axis perpendicular to the disc surface, i.e., a so-called fast axis (see FIG. 20 ).

[0145] [Wavelength-Selective Retardation Plate] The optical element 10 of the present invention includes a wavelength-selective retardation plate 18G provided between the first optically anisotropic member 12 and the second optically anisotropic member 14. In the optical element of the present invention, the wavelength-selective retardation plate is a member that converts circularly polarized light in a specific wavelength range into circularly polarized light with an opposite rotation direction. In the optical element shown in the figure, the wavelength-selective retardation plate 18G selectively converts circularly polarized green light into circularly polarized light with an opposite rotation direction, converting right-handed circularly polarized green light into left-handed circularly polarized green light and converting left-handed circularly polarized green light into right-handed circularly polarized green light, while transmitting (passing through) other light while maintaining its rotation direction.

[0146] In other words, a wavelength-selective retardation plate shifts the phase by π only in a specific wavelength range. Such a wavelength-selective retardation plate can also be called, for example, a λ / 2 plate that acts only in a specific wavelength range. The wavelength-selective retardation plate (optical element) is as described above.

[0147] [Function of Optical Element] As described above, an optically anisotropic layer formed using a composition containing a liquid crystal compound and having a liquid crystal orientation pattern in which the direction of the optical axis 30A rotates along the direction of arrow X refracts circularly polarized light, but the angle of refraction varies depending on the wavelength of the light. Specifically, the longer the wavelength of light, the greater the angle of refraction. Therefore, for example, when incident light is red, green, and blue light, red light is refracted most greatly and blue light is refracted least greatly. Therefore, for example, in an AR glass light guide plate, if an optical element made of an optically anisotropic layer having the above-mentioned liquid crystal orientation pattern in which the direction of the optical axis 30A rotates is used as a diffraction element for light entering and exiting the light guide plate, the transmission directions of red light, green light, and blue light will differ in a full-color image, resulting in an image with so-called color shift, in which the red image, green image, and blue image do not match. Here, color misalignment can be eliminated by providing a light guide plate corresponding to each of the red, green, and blue images and stacking three light guide plates, as described in, for example, Bernard C. Kress et al., Towards the Ultimate Mixed Reality Experience: HoloLens Display Architecture Choices, SID 2017 DIGEST, pp. 127-131. However, this configuration makes the light guide plates thick and heavy overall, and also makes the configuration complicated.

[0148] In contrast, the optical element of the present invention has an arrangement of multiple optically anisotropic layers, and a wavelength-selective retardation plate between at least one pair of adjacent optically anisotropic layers among the arranged optically anisotropic layers. Furthermore, the optically anisotropic layers have a liquid crystal orientation pattern in which the orientation of the optical axis derived from the liquid crystal compound rotates in one direction, and the period of the liquid crystal orientation pattern of at least one optically anisotropic layer is different from that of the other optically anisotropic layers. With such an optical element of the present invention, the wavelength dependence of the refraction angle of light is significantly reduced, and light of different wavelengths can be refracted in approximately the same direction and transmitted and emitted. Therefore, by using the optical element of the present invention (e.g., optical element 32 described below) as a diffraction element that introduces light into a light guide plate and / or a diffraction element that outputs light from the light guide plate in, for example, AR glasses, a single light guide plate can propagate red, green, and blue images without causing color shift, thereby displaying appropriate images to the user.

[0149] The operation of the optical element 10 will be described in detail below with reference to the conceptual diagrams of Figures 11 and 12. In the optical element of the present invention, the optical operation is basically achieved only by the optically anisotropic layer and the wavelength-selective retardation plate. Therefore, in order to simplify the drawings and clearly show the configuration and effects, Figure 11 (and Figure 12 , which will be described later) shows only the first optically anisotropic layer 26A and the second optically anisotropic layer 26B of the first optically anisotropic member 12 and the second optically anisotropic member 14, respectively, and the illustrated members are spaced apart in the arrangement direction.

[0150] As described above, the optical element 10 includes a wavelength-selective retardation plate 18G disposed between the first optically anisotropic member 12 having the first optically anisotropic layer 26A and the second optically anisotropic member 14 having the second optically anisotropic layer 26B, which reverses the rotation direction of circularly polarized green light. The optical element 10, as an example, refracts and transmits incident light, for example, circularly polarized blue light and circularly polarized green light. While the incident light in FIG. 11 is right-handed circularly polarized light, the same effect can be achieved if the incident light is left-handed circularly polarized light, except that the direction of refraction is reversed.

[0151] In the optical element 10, right-handed circularly polarized green light G R and right-handed circularly polarized blue light BR (Incident light L in FIG. 10 4 When the left-handed circularly polarized light G 1L and left-handed circularly polarized blue light B 1L (Transmitted light L in FIG. 10 5 As described above, the angle of refraction by the first optically anisotropic layer 26A is larger for green light having a longer wavelength, and therefore, as shown in FIG. 12, the angle of refraction for the incident light is the angle θ G1 The angle θ of blue light (B) B1 Furthermore, one period Λ of the optically anisotropic layer is larger than one period Λ of the first optically anisotropic layer 26A. A is shorter, the angle of refraction of each ray is larger than when it passes through the second optically anisotropic layer 26B.

[0152] Left-handed circularly polarized green light G transmitted through the first optically anisotropic layer 26A 1L and left-handed circularly polarized blue light B 1L Then, the left-handed circularly polarized light G of the green light is incident on the wavelength-selective retardation plate 18G. As described above, the wavelength-selective retardation plate 18G converts only the circularly polarized light of the green light into circularly polarized light of the opposite rotation direction, and transmits (straight passes through) the other light while maintaining the rotation direction. 1L and left-handed circularly polarized blue light B 1L is incident on the wavelength selective retardation plate 18G and passes through it, and is converted into left-handed circularly polarized blue light B 1L On the other hand, left-handed circularly polarized green light G 1L is right-handed circularly polarized green light G 1R is converted to

[0153] Right-handed circularly polarized green light G transmitted through the wavelength-selective retardation plate 18G 1R and left-handed circularly polarized blue light B 1L The right-handed circularly polarized green light G that has entered the second optically anisotropic layer 26B is then incident on the second optically anisotropic layer 26B. 1R and left-handed circularly polarized blue light B 1L is similarly refracted and converted into left-handed circularly polarized green light G 2L and right-handed circularly polarized blue light B2R and is emitted.

[0154] Here, right-handed circularly polarized green light G 1R and left-handed circularly polarized blue light B 1L As described above, the first optically anisotropic layer 26A and the second optically anisotropic layer 26B have opposite rotation directions of the optical axes 30A of the liquid crystal compounds 30. Therefore, as shown in FIGS. 11 and 12, left-handed circularly polarized light B of blue light is rotated in the opposite direction. 2L is further refracted in the direction opposite to the arrow X direction, and as shown on the left side of FIG. 12, the incident light (right-handed circularly polarized blue light B R ) with respect to the angle θ B2 On the other hand, right-handed circularly polarized green light G 1R 12, the left-handed circularly polarized light G of the green light is refracted in the direction of arrow X in the second optically anisotropic layer 26B, in the opposite direction to that of the first optically anisotropic layer 26A. 2L is the incident light (right-handed circularly polarized green light G R ) with the first angle θ G1 Left-handed circularly polarized blue light B 2L Angle θ B2 Almost the same as the angle θ G2 It is emitted at.

[0155] As described above, in the optical element 10 of the present invention, green light, which has a long wavelength and is highly refracted by the optically anisotropic layer, is refracted in the direction opposite to the arrow X by the first optically anisotropic layer 26A, and then refracted in the direction of arrow X by the second optically anisotropic layer 26B so as to return the refraction. On the other hand, blue light, which has a short wavelength and is less refracted by the optically anisotropic layer, is refracted in the direction opposite to the arrow X by both the first optically anisotropic layer 26A and the second optically anisotropic layer 26B. That is, in the optical element 10, depending on the magnitude of refraction by the optically anisotropic layer due to wavelength, long-wavelength light, which is highly refracted, is refracted the first time, and then refracted in the opposite direction the second time to return the refraction. On the other hand, short-wavelength light, which is less refracted, is refracted the second time in the same direction as the first time. As a result, the refraction angle θ of the green light with respect to the incident light is G2 and the angle of refraction of blue light θB2 Therefore, according to the optical element 10 of the present invention, the incident blue light and green light can be refracted at approximately the same angle and emitted in approximately the same direction.

[0156] As described above, the angle of light refracted by the first optically anisotropic layer 26A and the second optically anisotropic layer 26B increases as the wavelength of the light increases. Furthermore, the angle of light refracted by the first optically anisotropic layer 26A and the second optically anisotropic layer 26B increases as the period Λ of the optic axis 30A rotating by 180° along the direction of arrow X in the liquid crystal alignment pattern decreases. In the optical element 10, as shown in FIG. 6, for example, the period Λ of the liquid crystal alignment pattern in the first optically anisotropic layer 26A increases. A is one period Λ of the liquid crystal alignment pattern in the second optically anisotropic layer 26B. B That is, the first optically anisotropic layer 26A on the light incident side refracts light more strongly. Therefore, by adjusting one period Λ of the liquid crystal orientation pattern for the wavelength of light of interest, it is possible to suitably make the emission directions of light of different wavelengths the same.

[0157] When light of two wavelength ranges is targeted as in the illustrated optical element 10, the design wavelength of the long wavelength light is λa and the design wavelength of the short wavelength light is λb (λa>λb), and one period of the liquid crystal orientation pattern in the first optically anisotropic layer is Λ 1 , one period of the liquid crystal alignment pattern in the second optically anisotropic layer is represented by Λ 2 In this case, the following equation Λ 2 = [(λa+λb) / (λa-λb)]Λ 1 When the following expression is satisfied, the emission directions of light in the two wavelength ranges can be made to be substantially the same. In this expression, either the first optically anisotropic layer 26A or the second optically anisotropic layer 26B may be the first layer. Taking this into consideration, in the present invention, it is preferable that the optical element 10 intended for light of two wavelengths (wavelength ranges) satisfies the following expression: 0.6*{[(λa+λb) / (λa-λb)]Λ 1 ≦Λ 2 ≦3.0*{[(λa+λb) / (λa−λb)]Λ 1} This makes it possible to make the wavelength dependency of refraction extremely small, and to make the emission directions of light in the two wavelength ranges approximately the same. Furthermore, in the present invention, it is more preferable that the optical element 10 intended for light of two wavelengths (wavelength ranges) satisfies the following formula: 0.7*{[(λa+λb) / (λa-λb)]Λ 1 ≦Λ 2 ≦1.8*{[(λa+λb) / (λa−λb)]Λ 1} It is more preferable that the following formula is satisfied: 0.8*{[(λa+λb) / (λa-λb)]Λ 1 ≦Λ 2 ≦1.3*{[(λa+λb) / (λa−λb)]Λ 1} It is particularly preferable that the following formula is satisfied: 0.9*{[(λa+λb) / (λa-λb)]Λ 1 ≦Λ 2 ≦1.15*{[(λa+λb) / (λa−λb)]Λ 1}

[0158] <Second Aspect of Optical Element> The optical element 10 described above is intended for light in two wavelength ranges (design wavelengths), namely, green light and blue light, but the optical element of the present invention is not limited to this and may be intended for light in three or more wavelength ranges, and may refract and emit incident light.

[0159] An example is shown in Figure 13. Note that the optical element 32 shown in Figure 13 uses many of the same members as the optical element 10 shown in Figure 6, so the same members are denoted by the same reference numerals, and the following description will mainly focus on the different parts. The optical element 32 shown in Figure 13 has a third optical anisotropic member 16 and a wavelength-selective retardation plate 18R in addition to the first optical anisotropic member 12, second optical anisotropic member 14, and wavelength-selective retardation plate 18G of the optical element 10 described above.

[0160] The third optically anisotropic member 16 has a configuration similar to that of the first optically anisotropic member 12, etc., and includes a support 20, an alignment film 24C, and a third optically anisotropic layer 26C. The alignment film 24C and the third optically anisotropic layer 26C are similar to the alignment film 24A and the first optically anisotropic layer 26A described above, except for a different period Λ. The wavelength-selective retardation plate 18R selectively converts circularly polarized red light into circularly polarized light with the opposite rotation direction, converting right-handed circularly polarized red light into left-handed circularly polarized red light and converting left-handed circularly polarized red light into right-handed circularly polarized red light, while transmitting all other light as is.

[0161] In the optical element 32, the first optically anisotropic layer 26A and the third optically anisotropic layer 26C have the same rotation direction of the optical axis 30A of the liquid crystal compound 30 along the direction of arrow X, while the second optically anisotropic layer 26B has the opposite rotation direction of the optical axis 30A of the liquid crystal compound 30 along the direction of arrow X to that of the other two optically anisotropic layers. In the optical element 32, one period Λ in the direction of arrow X, in which the optical axis 30A of the liquid crystal compound 30 rotates by 180° in the liquid crystal orientation pattern, is equal to one period Λ of the first optically anisotropic layer 26A. A is the shortest, and one period Λ of the second optically anisotropic layer 26B is B is the longest. The optical element 32 has the first optically anisotropic member 12 side as the light incident side. That is, in the optical element 32, the first optically anisotropic layer 26A on the light incident side refracts light the most. Furthermore, the optical element 32 has a wavelength-selective retardation plate 18R disposed between the first optically anisotropic member 12 (first optically anisotropic layer 26A) and the second optically anisotropic member 14 (second optically anisotropic layer 26B) that selectively converts the rotation direction of circularly polarized light of red light. Furthermore, the optical element 32 has a wavelength-selective retardation plate 18G disposed between the second optically anisotropic member 14 and the third optically anisotropic member 16 (third optically anisotropic layer 26C) that selectively converts the rotation direction of circularly polarized light of green light.

[0162] The operation of the optical element 32 will be described in detail below with reference to Figures 14 and 15. The optical element 10 refracts and transmits incident light, for example, circularly polarized red light, circularly polarized green light, and circularly polarized blue light, in a predetermined direction. As in Figure 11 above, the incident light in Figure 14 is right-handed circularly polarized light, but the operation and effect are the same even if the incident light is left-handed circularly polarized light, except that the direction of refraction is reversed.

[0163] In the optical element 10, right-handed circularly polarized red light R R , right-handed circularly polarized green light G R and right-handed circularly polarized blue light B R (Incident light L in FIG. 10 4 When the left-handed circularly polarized light R 1L , left-handed circularly polarized green light G 1L and left-handed circularly polarized blue light B 1L (Transmitted light L in FIG. 10 5 As described above, the angle of refraction by the first optically anisotropic layer 26A is largest for red light, which has the longest wavelength, and smallest for blue light, which has the shortest wavelength. Therefore, the angle of refraction of the incident light is, as shown in FIG. 15, the angle θ R1 is the largest, and the angle θ of green light (G) G1 is in the middle, and the angle θ of blue light (B) B1 The period Λ of the optically anisotropic layer is the smallest. A is shortest, the angle of refraction of each ray is largest when it passes through the first optically anisotropic layer 26A.

[0164] Left-handed circularly polarized red light R transmitted through the first optically anisotropic layer 26A 1L , left-handed circularly polarized green light G 1L and left-handed circularly polarized blue light B 1L Next, the left-handed circularly polarized light R of the red light is incident on the wavelength-selective retardation plate 18R. As described above, the wavelength-selective retardation plate 18R converts only the circularly polarized light of the red light into circularly polarized light of the opposite rotation direction, and transmits the other light as it is. 1L , left-handed circularly polarized green light G 1Land left-handed circularly polarized blue light B 1L is incident on the wavelength selective retardation plate 18R and passes through it, and is converted into left-handed circularly polarized green light G 1L and left-handed circularly polarized blue light B 1L On the other hand, left-handed circularly polarized red light R 1L is right-handed circularly polarized red light R 1R is converted to

[0165] Right-handed circularly polarized red light R transmitted through the wavelength-selective retardation plate 18R 1R , left-handed circularly polarized green light G 1L and left-handed circularly polarized blue light B 1L The right-handed circularly polarized red light R then enters the second optically anisotropic layer 26B. 1R , left-handed circularly polarized green light G 1L and left-handed circularly polarized blue light B 1L is similarly refracted and converted into circularly polarized light of the opposite rotation direction, resulting in left-handed circularly polarized red light R 2L , right-handed circularly polarized green light G 2R and right-handed circularly polarized blue light B 2R and is emitted.

[0166] Here, both the green light and the blue light incident on the second optically anisotropic layer 26B are left-handed circularly polarized light. In contrast, the red light incident on the second optically anisotropic layer 26B is right-handed circularly polarized light whose circular polarization direction is different from that of the green light and the blue light, and whose direction of circular polarization has been converted by the wavelength-selective retardation plate 18R. As described above, the first optically anisotropic layer 26A and the second optically anisotropic layer 26B have opposite rotation directions of the optical axes 30A of the liquid crystal compounds 30. Therefore, as shown in Figures 14 and 15, the left-handed circularly polarized light G of the green light incident on the second optically anisotropic layer 26B 2L and left-handed circularly polarized blue light B 2L is further refracted in the direction opposite to the arrow X direction, and as shown in FIG. 15, the incident light (right-handed circularly polarized green light G R and right-handed circularly polarized blue light B R ) with respect to the angle θ G2 and angle θ B2 On the other hand, the right-handed circularly polarized light R of red light, which is incident on the second optically anisotropic layer 26B and has the opposite direction to the circularly polarized light R of red light, is emitted. 1R15, is refracted in the direction of arrow X so as to be returned to the first optically anisotropic layer 26A. As a result, the left-handed circularly polarized red light R emitted from the second optically anisotropic layer 26B is 2L is the incident light (right-handed circularly polarized red light R R ) with respect to the angle θ R1 Angle θ is smaller than R2 The period Λ of the optically anisotropic layer is equal to the period Λ of the second optically anisotropic layer 26B. B Since the angle of refraction of each ray is the smallest when it passes through the second optically anisotropic layer 26B, the angle of refraction of each ray is the smallest when it passes through the second optically anisotropic layer 26B.

[0167] Left-handed circularly polarized red light R transmitted through the second optically anisotropic layer 26B 2L , right-handed circularly polarized green light G 2R and right-handed circularly polarized blue light B 2R Next, the left-handed circularly polarized light R of the red light is incident on the wavelength-selective retardation plate 18G. As described above, the wavelength-selective retardation plate 18G converts only the circularly polarized light of the green light into circularly polarized light of the opposite rotation direction, and transmits the other light as it is. 2L , right-handed circularly polarized green light G 2R and right-handed circularly polarized blue light B 2R is incident on the wavelength selective retardation plate 18G and passes through it, and is converted into left-handed circularly polarized red light R 2L and right-handed circularly polarized blue light B 2R On the other hand, right-handed circularly polarized green light G 2R is left-handed circularly polarized green light G 2L is converted to

[0168] Left-handed circularly polarized red light R transmitted through the wavelength-selective retardation plate 18G 2L , left-handed circularly polarized green light G 2L and right-handed circularly polarized blue light B 2R The left-handed circularly polarized red light R that has entered the third optically anisotropic layer 26C is then incident on the third optically anisotropic layer 26C. 2L , left-handed circularly polarized green light G 2L and right-handed circularly polarized blue light B 2R is similarly refracted and converted into circularly polarized light of the opposite rotation direction, resulting in right-handed circularly polarized red light R 3R , right-handed circularly polarized green light G 3Rand left-handed circularly polarized blue light B 3L and is emitted.

[0169] Here, the blue light incident on the third optical anisotropic layer 26C is right-handed circularly polarized blue light B 2R In addition, since the direction of circular polarization of the red light has been converted by the wavelength selective retardation plate 18R in advance, the red light incident on the third optically anisotropic layer 26C is left-handed circularly polarized red light R, which has a different direction of circular polarization from that of the blue light. 2L Furthermore, the green light incident on the third optically anisotropic layer 26C is converted into left-handed circularly polarized green light G, the direction of which has been converted by the wavelength-selective retardation plate 18G. 2L That is, the blue light incident on the third optically anisotropic layer 26C is right-handed circularly polarized light, and the red and green lights are left-handed circularly polarized light whose circular polarization direction has been converted by the wavelength-selective retardation plate. As described above, the second and third optically anisotropic layers 26B and 26C have opposite rotation directions of the optical axes 30A of the liquid crystal compounds 30.

[0170] Therefore, as shown in FIGS. 14 and 15, the right-handed circularly polarized light B of blue light incident on the third optically anisotropic layer 26C 2R is further refracted in the direction opposite to the arrow X direction, and as shown in FIG. 15, the incident light (right-handed circularly polarized blue light B R ) with respect to the angle θ B3 In contrast, the left-handed circularly polarized red light R 2L When the light is incident on the third optically anisotropic layer 26C, it is further refracted so as to return in the direction of the arrow X. As a result, the right-handed circularly polarized red light R emitted from the third optically anisotropic layer 26C is 3R is the incident light (right-handed circularly polarized red light R R ) with respect to the angle θ R2 Angle θ is smaller than R3 Similarly, green light, which has the opposite circular polarization to blue light, is emitted as left-handed circularly polarized light G. 2L When the light enters the third optically anisotropic layer 26C, it is refracted in the direction of arrow X, as shown in the center of FIG. 14. As a result, the right-handed circularly polarized green light G 3R is the incident light (right-handed circularly polarized green light G R ) with respect to the angle θG2 Angle θ is smaller than G3 It is emitted at.

[0171] That is, in the optical element 32, red light, which has the longest wavelength and is refracted most by the optically anisotropic layers, is refracted in the direction opposite to the arrow X by the first optically anisotropic layer 26A, and then refracted twice in the opposite arrow X direction by the second optically anisotropic layer 26B and the third optically anisotropic layer 26C. Green light, which has the second longest wavelength and is refracted second most by the optically anisotropic layers, is refracted in the direction opposite to the arrow X by the first optically anisotropic layer 26A and the second optically anisotropic layer 26B, and then refracted once in the opposite arrow X direction by the third optically anisotropic layer 26C. Blue light, which has the shortest wavelength and is refracted least by the optically anisotropic layers, is refracted three times in the opposite arrow X direction by the first optically anisotropic layer 26A, the second optically anisotropic layer 26B, and the third optically anisotropic layer 26C. In this way, the optical element 32 of the present invention first refracts all light rays largely in the same direction, and then, depending on the magnitude of refraction by the optically anisotropic layer depending on the wavelength, refracts the light rays with the longest wavelengths the greatest number of times in a direction opposite to the initial refraction, reduces the number of times of refraction in the direction opposite to the initial refraction as the wavelength becomes shorter, and minimizes the number of times of refraction in the direction opposite to the initial refraction for the light rays with the shortest wavelengths. This allows the refraction angle θ of the red light with respect to the incident light to be adjusted. R3 and the angle of refraction of green light θ G3 and the angle of refraction of blue light θ B3 Therefore, according to the optical element 32 of the present invention, the incident red light, blue light, and green light can be refracted at approximately the same angle and emitted in approximately the same direction.

[0172] When light of three wavelength ranges is targeted as in the illustrated optical element 32, the design wavelength of the longest wavelength light is λa, the design wavelength of the intermediate wavelength light is λb, and the design wavelength of the shortest wavelength light is λc (λa>λb>λc), and one period of the liquid crystal orientation pattern in the first optically anisotropic layer is Λ. 1 , one period of the liquid crystal alignment pattern in the second optically anisotropic layer is represented by Λ 2 , one period of the liquid crystal alignment pattern in the third optically anisotropic layer is represented by Λ 3Then, the following two equations Λ 2 = [(λa+λc)λb / (λa-λb)λc]Λ 1 , Λ 3 = [(λa+λc)λb / (λb-λc)λa]Λ 1 When the following expression is satisfied, the emission directions of light in the two wavelength ranges can be made to be approximately the same. In this expression, either the first optically anisotropic layer 26A or the third optically anisotropic layer 26C may be the first layer. Taking this into consideration, in the present invention, in the optical element 32 intended for light of three wavelengths (wavelength ranges), it is preferable to satisfy at least one of the following two expressions, and more preferably to satisfy both: 0.6*{[(λa+λc)λb / (λa-λb)λc]Λ 1 ≦Λ 2 ≦3.0*{[(λa+λc)λb / (λa−λb)λc]Λ 1} 0.6*{[(λa+λc)λb / (λb-λc)λa]Λ 1 ≦Λ 3 ≦3.0*{[(λa+λc)λb / (λb−λc)λa]Λ 1} This makes it possible to make the wavelength dependency of refraction extremely small and make the emission directions of light in the two wavelength ranges approximately the same. Furthermore, in the present invention, it is more preferable that the optical element 32 intended for light of three wavelengths (wavelength ranges) satisfies the following two formulas: 0.7*{[(λa+λc)λb / (λa-λb)λc]Λ 1 ≦Λ 2 ≦1.8*{[(λa+λc)λb / (λa−λb)λc]Λ 1} 0.7*{[(λa+λc)λb / (λb-λc)λa]Λ 1 ≦Λ 3 ≦1.8*{[(λa+λc)λb / (λb−λc)λa]Λ 1} It is more preferable that the following two formulas are satisfied: 0.8*{[(λa+λc)λb / (λa-λb)λc]Λ 1 ≦Λ 2 ≦1.3*{[(λa+λc)λb / (λa−λb)λc]Λ 1} 0.8*{[(λa+λc)λb / (λb-λc)λa]Λ 1≦Λ 3 ≦1.3*{[(λa+λc)λb / (λb−λc)λa]Λ 1 It is particularly preferable that the following two formulas are satisfied: 0.9*{[(λa+λc)λb / (λa-λb)λc]Λ 1 ≦Λ 2 ≦1.15*{[(λa+λc)λb / (λa−λb)λc]Λ 1} 0.9*{[(λa+λc)λb / (λb-λc)λa]Λ 1 ≦Λ 3 ≦1.15*{[(λa+λc)λb / (λb−λc)λa]Λ 1}

[0173] In the optical element of the present invention, as described above, a plurality of optically anisotropic layers are arranged, and according to the wavelength of the light, the longer the wavelength of the light that is refracted by the optically anisotropic layers, the more times the light is refracted in the opposite direction to the first optically anisotropic layer, so that light of different wavelengths can be refracted at approximately the same angle and emitted in approximately the same direction. Therefore, in the optical element of the present invention, when a plurality of wavelength converting retardation layers are provided, it is preferable that the wavelength range of the light that converts circularly polarized light into the opposite rotation direction becomes gradually shorter in the arrangement direction of the optically anisotropic layers, as in the optical element 32 shown in Figures 13 and 14.

[0174] Furthermore, in the optical element of the present invention, it is easier to control the refraction of each light beam and make the refraction of each light beam uniform by increasing the refraction by the initial optically anisotropic layer, gradually refracting the light beams in the same direction thereafter, and then gradually returning the refraction to the opposite direction. Considering this point, as with the optical element 32 shown in Figures 13 and 14, it is preferable that the period Λ of the liquid crystal orientation pattern of the optically anisotropic layer located at the end of the alignment direction is shortest. In other words, it is preferable that the refraction by the optically anisotropic layer located at the end of the alignment direction is maximized. Note that in the optical element of the present invention, the period Λ of the liquid crystal orientation pattern of the optically anisotropic layer may be configured to gradually increase in the alignment direction of the optically anisotropic layer. Alternatively, the period Λ of the liquid crystal orientation pattern of the optically anisotropic layer may vary irregularly in the alignment direction of the optically anisotropic layer, for example, by providing an optically anisotropic layer having an intermediate period Λ of the liquid crystal orientation pattern between an optically anisotropic layer having the largest period Λ of the liquid crystal orientation pattern and an optically anisotropic layer having the smallest period Λ of the liquid crystal orientation pattern, as in the optical element 32 shown in Figures 13 and 14. That is, in the optical element of the present invention, the period Λ of the liquid crystal orientation pattern of each optically anisotropic layer may be set appropriately depending on the wavelength of light and the refractive index of the optically anisotropic layer.

[0175] In the optical element of the present invention, when multiple wavelength-converting retardation layers are included, the optically anisotropic layers and the wavelength-converting retardation layers are basically arranged alternately, as in the optical element 32 shown in Figures 13 and 14. In this case, it is preferable that the number of wavelength-converting retardation layers is one less than the number of optically anisotropic layers. However, the present invention is not limited thereto. For example, multiple optically anisotropic layers may be arranged in succession, and light refracted continuously by the multiple optically anisotropic layers may be incident on the wavelength-converting retardation layer. Furthermore, multiple wavelength-converting retardation layers may be arranged between two optically anisotropic layers. However, when multiple wavelength-converting retardation layers that convert circularly polarized light in the same wavelength range into circularly polarized light with an opposite rotation direction are arranged between two optically anisotropic layers, it is preferable that the number of wavelength-converting retardation layers be an odd number.

[0176] In the optical element of the present invention, optically anisotropic layers may exist in which the period Λ of the liquid crystal alignment pattern is the same, but it is preferable that the period Λ of the liquid crystal alignment pattern is different in all optically anisotropic layers in order to easily make the refraction of light in a plurality of wavelength ranges, i.e., the emission angle, uniform.

[0177] In the optical element of the present invention, there is no limitation on one period Λ in the alignment pattern of the optically anisotropic layer, and it may be set appropriately depending on the application of the optical element, etc.

[0178] The optical element of the present invention may have a wavelength-selective retardation plate that selectively converts circularly polarized light of the shortest design wavelength into circularly polarized light with the opposite rotation direction. For example, a third wavelength-selective retardation plate B that selectively converts circularly polarized light of blue light into circularly polarized light with the opposite rotation direction may be disposed after the third optically anisotropic layer 26C (downstream in the light traveling direction). As described above, the third wavelength-selective retardation plate B converts only circularly polarized light of blue light into circularly polarized light with the opposite rotation direction, and transmits other light as it is. Therefore, right-handed circularly polarized light R of red light 3R , right-handed circularly polarized green light G 3R and left-handed circularly polarized blue light B 3L is incident on the third wavelength selective retardation plate B and passes through it, and is converted into right-handed circularly polarized red light R 3R and right-handed circularly polarized green light G 3R On the other hand, left-handed circularly polarized blue light B 3L is right-handed circularly polarized blue light B 3R As a result, the circularly polarized blue, green, and red light emitted from the optical element can be converted into circularly polarized light with the same rotation direction.

[0179] Here, the optical element of the present invention is suitably used, for example, in AR glasses as a diffraction element that refracts light displayed by a display and introduces it into a light guide plate, and as a diffraction element that refracts light propagating through the light guide plate and emits it from the light guide plate to a user's observation position. In particular, the optical element 32 capable of displaying full-color images is suitably used as a diffraction element in AR glasses. In this case, in order to achieve total internal reflection by the light guide plate, it is necessary to refract the light at a relatively large angle relative to the incident light and introduce it into the light guide plate. Furthermore, in order to reliably emit light that has propagated through the light guide plate, it is necessary to refract the light at a relatively large angle relative to the incident light. Furthermore, as described above, the angle of light transmission through the optically anisotropic layer can be increased by shortening the period Λ of the liquid crystal orientation pattern.

[0180] In consideration of this point, one period Λ of the liquid crystal alignment pattern of the optically anisotropic layer is preferably 50 μm or less, more preferably 10 μm or less, and even more preferably 3 μm or less. In consideration of the accuracy of the liquid crystal alignment pattern, one period Λ of the liquid crystal alignment pattern of the optically anisotropic layer is preferably 0.1 μm or more.

[0181] 9 to 15, the optical axis 30A of the liquid crystal compound 30 in the liquid crystal alignment pattern of the optically anisotropic layer continuously rotates only along the direction of the arrow X. However, the present invention is not limited to this, and various configurations can be used as long as the optical axis 30A of the liquid crystal compound 30 in the optically anisotropic layer continuously rotates along one direction.

[0182] One example is an optically anisotropic layer 34 having a liquid crystal orientation pattern that is a concentric pattern from the inside to the outside, in which the direction of the optical axis of the liquid crystal compound 30 changes while continuously rotating, as conceptually shown in the plan view of Fig. 17. In other words, the liquid crystal orientation pattern of the optically anisotropic layer 34 shown in Fig. 17 is a liquid crystal orientation pattern in which the direction of the optical axis of the liquid crystal compound 30 changes while continuously rotating is provided radially from the center of the optically anisotropic layer 34.

[0183] 17 shows only the liquid crystal compound 30 on the surface of the alignment film, as in FIG. 9 . However, as described above, the optically anisotropic layer 34 has a structure in which the liquid crystal compound 30 is stacked starting from the liquid crystal compound 30 on the surface of the alignment film, as shown in FIG. 7 . Furthermore, although FIG. 17 shows only one optically anisotropic layer 34, the optical element of the present invention has a plurality of optically anisotropic layers, and has a wavelength-selective retardation plate between at least one pair of optically anisotropic layers, as described above. Therefore, even when an optically anisotropic layer having such a concentric liquid crystal alignment pattern is included, the optical element has a configuration in which a first optically anisotropic layer, a wavelength-selective retardation plate that converts circularly polarized light of red light, a second optically anisotropic layer, a wavelength-selective retardation plate that converts circularly polarized light of green light, and a third optically anisotropic layer are arranged, as in the optical element 32 shown in FIG. 13 .

[0184] In the optically anisotropic layer 34 shown in FIG. 17 , the optical axis (not shown) of the liquid crystal compound 30 is the longitudinal direction of the liquid crystal compound 30. In the optically anisotropic layer 34, the direction of the optical axis of the liquid crystal compound 30 changes while continuously rotating along a number of directions from the center of the optically anisotropic layer 34 toward the outside, for example, the direction indicated by arrow A1, the direction indicated by arrow A2, the direction indicated by arrow A3, etc. Circularly polarized light incident on the optically anisotropic layer 34 having this liquid crystal orientation pattern undergoes a change in absolute phase in each of the local regions where the optical axis direction of the liquid crystal compound 30 is different. At this time, the amount of change in each absolute phase differs depending on the direction of the optical axis of the liquid crystal compound 30 into which the circularly polarized light is incident.

[0185] The optically anisotropic layer 34 having such a concentric liquid crystal orientation pattern, i.e., a liquid crystal orientation pattern in which the optical axis changes by continuously rotating radially, can transmit incident light as divergent or convergent light depending on the rotation direction of the optical axis of the liquid crystal compound 30 and the direction of the incident circularly polarized light. That is, by making the liquid crystal orientation pattern of the optically anisotropic layer concentric, the optical element of the present invention can function as, for example, a convex lens or a concave lens.

[0186] Here, when the liquid crystal orientation pattern of the optically anisotropic layer is concentric and the optical element functions as a convex lens, it is preferable to gradually shorten one period Λ, in which the optical axis rotates 180°, from the center of the optically anisotropic layer 34 toward the outside in one direction in which the optical axis continuously rotates. As described above, the angle of refraction of light with respect to the incident direction increases as one period Λ of the liquid crystal orientation pattern becomes shorter. Therefore, by gradually shortening one period Λ of the liquid crystal orientation pattern from the center of the optically anisotropic layer 34 toward the outside in one direction in which the optical axis continuously rotates, the light focusing power of the optically anisotropic layer 34 can be further improved, and the performance as a convex lens can be improved.

[0187] In the present invention, depending on the application of the optical element, for example, when it is used as a concave lens, it is preferable to rotate one period Λ, in which the optical axis rotates by 180°, from the center of the optically anisotropic layer 34 in the opposite direction to the direction in which the optical axis continuously rotates, and gradually shorten the period Λ from the center of the optically anisotropic layer 34 toward the outside in one direction. As described above, the angle of refraction of light with respect to the incident direction increases as the period Λ in the liquid crystal orientation pattern becomes shorter. Therefore, by gradually shortening one period Λ in the liquid crystal orientation pattern from the center of the optically anisotropic layer 34 toward the outside in one direction in which the optical axis continuously rotates, the light divergence power of the optically anisotropic layer 34 can be further improved, and the performance as a concave lens can be improved.

[0188] In the present invention, it is also preferable to reverse the rotation direction of the incident circularly polarized light, for example, when the optical element is a concave lens.

[0189] In the present invention, when the optical element is used as a convex lens or a concave lens, it is preferable that the following formula be satisfied: Φ(r)=(π / λ)[(r 2 +f 2 ) 1/2 -f] where r is the distance from the center of the concentric circle and is expressed by the following formula: r = (x 2 +y 2 ) 1/2x and y represent the position in the plane, and (x, y) = (0, 0) represents the center of the concentric circle. Φ(r) represents the angle of the optical axis at the distance r from the center, λ represents the wavelength, and f represents the designed focal length.

[0190] Conversely, in the present invention, the period Λ of the concentric liquid crystal orientation pattern may be gradually increased from the center of the optically anisotropic layer 34 outward in one direction in which the optical axis continuously rotates. Furthermore, depending on the application of the optical element, for example, when it is desired to provide a light intensity distribution to transmitted light, a configuration may be used in which, rather than gradually changing the period Λ in one direction in which the optical axis continuously rotates, there are regions in which the period Λ varies partially in one direction in which the optical axis continuously rotates. In addition, the optical element of the present invention may have an optically anisotropic layer in which the period Λ is uniform throughout and an optically anisotropic layer in which there are regions in which the period Λ varies. In this regard, the same applies to a configuration in which the optical axis continuously rotates in only one direction, as shown in Figure 6, which will be described later.

[0191] 18 conceptually shows an example of an exposure device for forming such a concentric alignment pattern on an alignment film (e.g., alignment film 24A, alignment film 24B, and alignment film 24C). Exposure device 80 includes a light source 84 equipped with a laser 82, a polarizing beam splitter 86 that splits laser light M from laser 82 into S-polarized light MS and P-polarized light MP, a mirror 90A arranged in the optical path of the P-polarized light MP, a mirror 90B arranged in the optical path of the S-polarized light MS, a lens 92 arranged in the optical path of the S-polarized light MS, a polarizing beam splitter 94, and a λ / 4 plate 96.

[0192] The P-polarized light MP split by the polarizing beam splitter 86 is reflected by a mirror 90A and enters a polarizing beam splitter 94. On the other hand, the S-polarized light MS split by the polarizing beam splitter 86 is reflected by a mirror 90B, collected by a lens 92, and enters the polarizing beam splitter 94. The P-polarized light MP and the S-polarized light MS are combined by the polarizing beam splitter 94 and converted into right- and left-circularly polarized light according to the polarization direction by a λ / 4 plate 96, and then enter the alignment film 24 on the support 20. Here, due to interference between the right- and left-circularly polarized light, the polarization state of the light irradiated onto the alignment film 24 changes periodically in the form of interference fringes. Because the crossing angle between the left- and right-circularly polarized light changes from the inside to the outside of the concentric circles, an exposure pattern whose pitch changes from the inside to the outside is obtained. As a result, a concentric alignment pattern in which the alignment state changes periodically is obtained on the alignment film 24.

[0193] In this exposure device 80, one period Λ of the liquid crystal orientation pattern in which the optical axis of the liquid crystal compound 30 continuously rotates 180° along one direction can be controlled by changing the refractive power of the lens 92 (the F-number of the lens 92), the focal length of the lens 92, and the distance between the lens 92 and the orientation film 24. Furthermore, by adjusting the refractive power of the lens 92 (the F-number of the lens 92), the length Λ of one period of the liquid crystal orientation pattern can be changed in one direction in which the optical axis continuously rotates. Specifically, the length Λ of one period of the liquid crystal orientation pattern in one direction in which the optical axis continuously rotates can be changed by adjusting the spread angle of the light expanded by the lens 92, which interferes with the parallel light. More specifically, when the refractive power of the lens 92 is weakened, the light approaches parallel light, so the length Λ of one period of the liquid crystal orientation pattern gradually shortens from the inside to the outside, and the F-number increases. Conversely, when the refractive power of the lens 92 is increased, the length Λ of one period of the liquid crystal alignment pattern suddenly decreases from the inside to the outside, and the F-number decreases.

[0194] In this way, the configuration in which the period Λ of the optical axis, which rotates 180°, is changed in one direction in which the optical axis continuously rotates, can also be used in the configuration in which the optical axis 30A of the liquid crystal compound 30 continuously rotates and changes only in one direction, the direction of the arrow X, as shown in Figures 6 to 15. For example, by gradually shortening the period Λ of the liquid crystal orientation pattern in the direction of the arrow X, an optical element that transmits light in a condensing manner can be obtained. Furthermore, by reversing the direction in which the optical axis rotates 180° in the liquid crystal orientation pattern, an optical element that transmits light in a diffusive manner only in the direction of the arrow X can be obtained. Note that an optical element that transmits light in a diffusive manner only in the direction of the arrow X can also be obtained by reversing the rotation direction of the incident circularly polarized light. Furthermore, depending on the application of the optical element, for example, when it is desired to provide a light intensity distribution in the transmitted light, a configuration in which the period Λ is partially different in the direction of the arrow X rather than gradually changing the period Λ in the direction of the arrow X can also be used. For example, as a method for partially changing one period Λ, a method of patterning a photo-alignment film by scanning exposure while arbitrarily changing the polarization direction of focused laser light can be used.

[0195] The optical element of the present invention can be used in various applications that transmit light in a direction different from the incident direction, such as an optical path changing member in an optical device, a light focusing element, a light diffusing element in a predetermined direction, and a diffraction element.

[0196] As a preferred example, as conceptually shown in FIG. 19 , the optical element 32 may be provided at a distance from the light guide plate 42. This diffractive element guides light (projected image) emitted by the display 40 into the light guide plate 42 at an angle sufficient for total reflection, and then emits the light propagating through the light guide plate 42 to a viewing position for a user U of the AR glasses. While FIG. 19 illustrates the optical element 32 shown in FIG. 13 as a full-color image, the optical element 10 shown in FIG. 6 may also be suitably used when displaying a two-color image with AR glasses. As described above, the optical element of the present invention has a small angle dependency of the refraction angle during transmission, allowing red, green, and blue light emitted by the display 40 to be refracted in the same direction. Therefore, even when red, green, and blue images are propagated through a single light guide plate 42, a full-color image without color shift can be emitted from the light guide plate to a viewing position for a user U of the AR glasses. Therefore, by using the optical element of the present invention, the light guide plate of the AR glass can be made thinner and lighter overall, and the configuration of the AR glass can be simplified. Note that the light guide element of the present invention is not limited to a configuration in which two optical elements of the present invention are provided spaced apart from each other on a light guide plate 42 as shown in Figure 19, but may be a configuration in which only one optical element of the present invention is provided on a light guide plate for introducing light into the light guide plate 42 or for extracting light from the light guide plate 42.

[0197] In the above examples, the optical element of the present invention is used as an optical element having two or three optically anisotropic layers, which transmits and refracts two colors of light, green light and blue light, or three colors of light, red light, green light, and blue light. However, the present invention is not limited to this, and various configurations can be used. For example, the optical element of the present invention may have three optically anisotropic layers and two wavelength-selective retardation plates, as in FIG. 13, and may transmit and refract two colors selected from red light, green light, and blue light, as well as infrared light or ultraviolet light. Alternatively, the optical element of the present invention may have four or five (or six or more) optically anisotropic layers and three or four (the number of optically anisotropic layers minus one) wavelength-selective retardation plates, and may transmit and refract infrared light and / or ultraviolet light in addition to red light, green light, and blue light. Alternatively, the optical element of the present invention may have two optically anisotropic layers and one wavelength-selective retardation plate, as in Fig. 6, and may be configured to transmit and refract red light and blue light or red light and green light, or to refract and transmit one color selected from red light, green light, and blue light, and infrared light or ultraviolet light, or to refract and transmit infrared light and / or ultraviolet light.

[0198] The present invention will be described in more detail below with reference to the following examples. The materials, amounts used, ratios, treatment details, and treatment procedures shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be construed as being limited by the following examples.

[0199] Example 1 Synthesis of Polymer PA-1 Having Photoalignable Groups According to the method described in Langmuir, 32(36), 9245-9253, (2016), the following monomer m-1 was synthesized using 2-hydroxyethyl methacrylate (HEMA) (Tokyo Chemical Industry Co., Ltd.) and the following cinnamic acid chloride derivative.

[0200] Cinnamic acid chloride derivatives

[0201] Monomer m-1

[0202] A flask equipped with a condenser, thermometer, and stirrer was charged with 5 parts by mass of 2-butanone as a solvent, and refluxed by heating in a water bath while flowing nitrogen into the flask at 5 mL / min. A solution containing 5 parts by mass of monomer m-1, 5 parts by mass of Cyclomer M100 (3,4-epoxycyclohexylmethyl methacrylate, manufactured by Daicel Corporation), 1 part by mass of 2,2'-azobis(isobutyronitrile) as a polymerization initiator, and 5 parts by mass of 2-butanone as a solvent was added dropwise over 3 hours and stirred for an additional 3 hours while maintaining reflux. After completion of the reaction, the mixture was allowed to cool to room temperature and diluted with 30 parts by mass of 2-butanone to obtain a polymer solution of approximately 20% by mass. The resulting polymer solution was poured into a large excess of methanol to precipitate the polymer, and the recovered precipitate was filtered, washed with a large amount of methanol, and then dried with air at 50 °C for 12 hours to obtain polymer PA-1 (see below) having a photoalignable group. The resulting polymer PA-1 had an epoxy equivalent of 396 g / eq and a weight average molecular weight of 28,000.

[0203]

[0204] [Preparation of Photo-Alignment Film P-1] The following composition for forming a photo-alignment film, PC-1, was continuously applied onto a commercially available triacetyl cellulose film "Z-TAC" (manufactured by Fujifilm Corporation) using a #2.4 wire bar. The support on which the coating film was formed was dried with hot air at 140°C for 120 seconds, and then irradiated with polarized ultraviolet light (10 mJ / cm). 2 , using an ultra-high pressure mercury lamp) to form a photo-alignment film P-1.

[0205] ---------------------------------------------------------------- Composition PC-1 for forming a photoalignment film ------------------------------------------------ Polymer PA-1 above 100.00 parts by mass Thermal acid generator PAG below 5.00 parts by mass Isopropyl alcohol 16.50 parts by mass Butyl acetate 1072.00 parts by mass Methyl ethyl ketone 268.00 parts by mass

[0206] Thermal acid generator PAG

[0207] [Formation of Optical Film A] The following polymerizable liquid crystal composition 1 was applied onto the photo-alignment film P-1 using a #13 wire bar. After heating at 110°C for 100 seconds, the composition layer was irradiated with ultraviolet light (irradiation dose: 500 mJ / cm) using a metal halide lamp (manufactured by Eye Graphics Co., Ltd.) at 55°C under a nitrogen atmosphere. 2 The orientation of the liquid crystal compound was fixed to form an optically anisotropic film A1. Subsequently, the following polymerizable liquid crystal composition 2 was applied to the optically anisotropic film A1 using a #16 wire bar, heated at 110°C for 100 seconds, and then irradiated with ultraviolet light using a metal halide lamp at 55°C under a nitrogen atmosphere (irradiation dose: 500 mJ / cm). 2 The process from application of the polymerizable liquid crystal composition 2 described below to ultraviolet irradiation was repeated three more times to form an optically anisotropic film A2. Furthermore, the polymerizable liquid crystal composition 3 described below was applied onto the optically anisotropic film A2 using a #13 wire bar, and the film was heated at 110°C for 100 seconds. After that, the composition layer was irradiated with ultraviolet light (irradiation dose: 500 mJ / cm) using a metal halide lamp at 55°C under a nitrogen atmosphere. 2), and optically anisotropic film A3 was formed. As a result of the above, an optical film A was prepared in which the support / photo-alignment film P-1 / optically anisotropic film A1 / optically anisotropic film A2 / optically anisotropic film A3 were laminated in this order. In the prepared optical film A, the optically anisotropic film A1 and the optically anisotropic film A3 correspond to the λ / 4 plate. Furthermore, the optically anisotropic film A2 corresponds to the liquid crystal polarization interference element 216 shown in FIG. 1. Therefore, the prepared optical film A corresponds to the above-mentioned optical element. Furthermore, each layer constituting the optical film A was a layer in which the orientation state of the liquid crystal compound was fixed as shown in Table 1 below. Furthermore, the retardation of each layer constituting the optical film A is also shown in Table 1 below.

[0208] ------------------------------------------------ Polymerizable liquid crystal composition 1------------------------------------------------ Liquid crystal compound A-1 (weight average molecular weight 20,000) below: 67 parts by mass Liquid crystal compound B-1 below: 33 parts by mass Polymerization initiator S-1 below: 3 parts by mass Chiral agent A below: 0.40 parts by mass Chiral agent B below: 0.65 parts by mass Leveling agent (compound L-1 below): 0.15 parts by mass Vertical alignment assistant (compound T-1 below): 0.2 parts by mass Cyclohexanone 516.8 parts by mass------------------------------------------------

[0209] Liquid crystal compound A-1

[0210] Liquid crystal compound B-1

[0211] Polymerization initiator S-1

[0212] Chiral Agent A

[0213] Chiral Agent B

[0214] Compound L-1

[0215] Compound T-1

[0216] When the polymerizable liquid crystal composition 2 is applied, the liquid crystal compound A-1 (rod-shaped liquid crystal compound) is concentrated on the air interface side, and the liquid crystal compound B-1 (discosmic liquid crystal compound) is concentrated on the side opposite the air interface side. That is, the composition separates from the photo-alignment film P-1 side into a layer containing a discotic liquid crystal compound and a layer containing a rod-shaped liquid crystal compound. The chiral dopant A and the chiral dopant B are present in each of the separated layers, and the chiral dopant A exerts a right-handed helical twisting force on the discotic liquid crystal compound and the rod-shaped liquid crystal compound. On the other hand, the chiral dopant B exerts a left-handed helical twisting force only on the rod-shaped liquid crystal compound. As a result, the layer containing the discotic liquid crystal compound exhibits a right-handed twist, and the layer containing the rod-shaped liquid crystal compound exhibits a left-handed twist, forming an optically anisotropic layer A2 as shown in Table 1 below.

[0217] ------------------------------------------------ Polymerizable liquid crystal composition 2---------------------------------------------------------------- 50 parts by mass of the liquid crystal compound A-1 (weight average molecular weight 20,000) 50 parts by mass of the liquid crystal compound B-1 3 parts by mass of the polymerization initiator S-1 0.05 parts by mass of the chiral agent A 0.19 parts by mass of the chiral agent B 0.15 parts by mass of leveling agent (compound L-1) 0.15 parts by mass of vertical alignment assistant (compound T-1) 0.2 parts by mass Cyclohexanone 516.8 parts by mass

[0218] ------------------------------------------------ Polymerizable liquid crystal composition 3 -------------------------------------------------- 33 parts by mass of the above liquid crystal compound A-1 (weight average molecular weight 20,000) 67 parts by mass of the above liquid crystal compound B-1 3 parts by mass of the above polymerization initiator S-1 0.07 parts by mass of the above chiral agent A 0.58 parts by mass of the following chiral agent C Leveling agent (above compound L-1) 0.15 parts by mass Vertical alignment assistant (above compound T-1) 0.2 parts by mass Cyclohexanone 516.8 parts by mass ------------------------------------------------

[0219] Chiral Agent C

[0220] Example 2 Optical film B was prepared in the same manner as in Example 1, except that the amounts of chiral dopants A, B, and C in the polymerizable liquid crystal composition and the diameter of the wire bar were changed. That is, optical film B was prepared by laminating support / photo-alignment film P-1 / optically anisotropic film B1 / optically anisotropic film B2 / optically anisotropic film B3 in this order. Optically anisotropic film B1, optically anisotropic film B2, and optically anisotropic film B3 correspond to the λ / 4 plate, the liquid crystal polarization interference element 216 shown in FIG. 1, and the λ / 4 plate, respectively, and optical film B corresponds to the above-mentioned optical element. When optical film B was prepared, the conditions were adjusted to obtain a retardation as shown in Table 2 below. Note that each layer constituting optical film B was a layer in which the alignment state of a liquid crystal compound was fixed as shown in Table 2 below.

[0221] Example 3 An optical film C was prepared in the same manner as in Example 1, except that the amounts of chiral dopants A, B, and C in the polymerizable liquid crystal composition and the diameter of the wire bar were changed. That is, an optical film C was prepared in which the support / photo-alignment film P-1 / optically anisotropic film C1 / optically anisotropic film C2 / optically anisotropic film C3 were laminated in this order. The optically anisotropic film C1, the optically anisotropic film C2, and the optically anisotropic film C3 correspond to the λ / 4 plate, the liquid crystal polarization interference element 216 shown in FIG. 1, and the λ / 4 plate, respectively, and the optical film C corresponds to the above-mentioned optical element. When preparing the optical film C, the conditions were adjusted to obtain a retardation as shown in Table 3 below. Note that each layer constituting the optical film C was a layer in which the alignment state of the liquid crystal compound was fixed as shown in Table 3 below.

[0222] Example 4 First, a film in which a support / photo-alignment film P-1 was laminated was prepared in the same manner as in Example 1.

[0223] (Formation of Optical Film D) The following polymerizable liquid crystal composition 4 was applied onto the photo-alignment film P-1 using a #4 wire bar. After heating at 100°C for 80 seconds, the composition layer was irradiated with ultraviolet light (irradiation dose: 19 mJ / cm) using a 365 nm LED lamp (manufactured by Acroedge Co., Ltd.) at 40°C in oxygen-containing air (oxygen concentration: approximately 20% by volume). 2 Subsequently, the obtained composition layer was heated at 90°C for 10 seconds, and then irradiated with ultraviolet light using a metal halide lamp at 55°C under a nitrogen atmosphere (irradiation dose: 500 mJ / cm 2 ), and the alignment of the liquid crystal compound was fixed to form an optically anisotropic film 4. Subsequently, the following polymerizable liquid crystal composition 5 was applied to the optically anisotropic film 4 using a #7 wire bar, heated at 100°C for 80 seconds, and then irradiated with ultraviolet light using a 365 nm LED lamp at 40°C in an oxygen-containing atmosphere (irradiation dose: 35 mJ / cm 2). The above-mentioned UV irradiation caused polymerization to proceed only on the side of the composition layer opposite to the air interface side, and deactivated the chiral agent C contained on the air interface side. The obtained composition layer was heated at 90°C for 10 seconds, and then irradiated with UV light using a metal halide lamp under a nitrogen atmosphere at 55°C. That is, polymerization of the entire composition layer was allowed to proceed while the twist direction of the liquid crystal compound in the composition layer on the air interface side was reversed to that of the layer on the opposite side to the air interface side. The process from applying the following polymerizable liquid crystal composition 5 to applying UV light using a metal halide lamp was repeated three more times to form an optically anisotropic film 5. Furthermore, the following polymerizable liquid crystal composition 6 was applied to the optically anisotropic film 5 using a #4 wire bar. After heating at 100°C for 80 seconds, the composition layer was irradiated with UV light using a 365 nm LED lamp at 40°C under an oxygen-containing atmosphere (irradiation dose: 38 mJ / cm). 2 Subsequently, the obtained composition layer was heated at 90°C for 10 seconds, and then irradiated with ultraviolet light using a metal halide lamp at 55°C under a nitrogen atmosphere (irradiation dose: 500 mJ / cm 2 ), and the alignment of the liquid crystal compound was fixed to form optically anisotropic film 6. As a result, optical film D was prepared, which was laminated in the following order: support / photo-alignment film P-1 / optically anisotropic film 4 / optically anisotropic film 5 / optically anisotropic film 6. In the prepared optical film D, optically anisotropic film 4 and optically anisotropic film 6 correspond to the λ / 4 plate. Furthermore, optically anisotropic film 5 corresponds to the liquid crystal polarization interference element 216 shown in FIG. 1. Therefore, the prepared optical film D corresponds to the above-mentioned optical element. Furthermore, each layer constituting the prepared optical film D was a layer in which the alignment state of the liquid crystal compound was fixed, as shown in Table 4 below. Furthermore, the retardation of each layer of optical film D is also shown in Table 4 below.

[0224] ------------------------------------------------ Polymerizable liquid crystal composition 4 -------------------------------------------------- 80 parts by mass of rod-shaped liquid crystal compound A described below 3 parts by mass of rod-shaped liquid crystal compound B described below 17 parts by mass of rod-shaped liquid crystal compound C described below Ethylene oxide-modified trimethylolpropane triacrylate (V#360, manufactured by Osaka Organic Chemical Industry Co., Ltd.) 4 parts by mass of polymerization initiator S-1 described above 3 parts by mass of chiral agent B described above 0.24 parts by mass of chiral agent C described above 0.55 parts by mass of leveling agent (compound L-1 described above) 0.08 parts by mass of methyl isobutyl ketone 36 parts by mass of ethyl propionate 71 parts by mass of methyl ethyl ketone 36 parts by mass

[0225] Rod-shaped liquid crystal compound A (a mixture of the following compounds):

[0226] Rod-shaped liquid crystal compound B

[0227] Rod-shaped liquid crystal compound C

[0228] ------------------------------------------------ Polymerizable Liquid Crystal Composition 5 ------------------------------------------------------------------ Rod-shaped liquid crystal compound A 80 parts by mass Rod-shaped liquid crystal compound B 3 parts by mass Rod-shaped liquid crystal compound C 17 parts by mass Ethylene oxide modified trimethylolpropane triacrylate (V#360, Osaka Organic Chemical Industry Co., Ltd.) 4 parts by mass Polymerization initiator S-1 3 parts by mass Chiral agent B 0.08 part by mass Chiral agent C 0.11 parts by mass Leveling agent (compound L-1) 0.08 part by mass Methyl isobutyl ketone 36 parts by mass Ethyl propionate 71 parts by mass Methyl ethyl ketone 36 parts by mass

[0229] ------------------------------------------------ Polymerizable Liquid Crystal Composition 6 ------------------------------------------------------------------ Rod-shaped liquid crystal compound A 80 parts by mass Rod-shaped liquid crystal compound B 3 parts by mass Rod-shaped liquid crystal compound C 17 parts by mass Ethylene oxide-modified trimethylolpropane triacrylate (V#360, manufactured by Osaka Organic Chemical Industry Co., Ltd.) 4 parts by mass Polymerization initiator S-1 3 parts by mass Chiral agent B 0.12 parts by mass Chiral agent D below 0.94 parts by mass Leveling agent (compound L-1 above) 0.08 parts by mass Methyl isobutyl ketone 36 parts by mass Ethyl propionate 71 parts by mass Methyl ethyl ketone 36 parts by mass

[0230] Chiral Agent D

[0231] <Measurement of Optical Properties> The optical properties of the optical films A to D prepared above were determined using an Axoscan from Axometrics and their analysis software (Multi-Layer Analysis). The alignment axis angle of the liquid crystal compound was measured from the opposite side of the substrate, with the longitudinal direction of the film being taken as the reference angle of 0°, and expressed as negative for clockwise (right-handed) and positive for counterclockwise (left-handed). The twist angle of the liquid crystal compound was measured by observing the optical film from the opposite side of the substrate, and the twist angle was expressed as negative when the alignment direction of the liquid crystal compound on the air side (near side) was clockwise (right-handed) and positive when it was counterclockwise (left-handed) relative to the alignment direction of the liquid crystal compound on the support side (rear side).

[0232]

[0233]

[0234]

[0235]

[0236] <Preparation of Circular Polarizers> In order to evaluate the wavelength dependence of transmission, which will be described later, circular polarizers B, G, and R were prepared as follows. First, circular polarizer G was prepared. First, a support similar to that in Example 1 was prepared.

[0237] [Formation of Orientation Film P-10] The following coating solution for forming the orientation film P-10 was continuously applied onto the support using a #2.4 wire bar. The support on which the coating film of the coating solution for forming the orientation film P-10 had been formed was dried on a hot plate at 80°C for 5 minutes to form the orientation film P-10.

[0238] ―――――――――――――――――――――――――――――――― Coating liquid for forming alignment film P-10 ―――――――――――――――――――――――――――――――― ・Material for photo alignment Polymer A2 4.35 parts by mass ・Low molecular compound B2 0.80 parts by mass ・Crosslinking agent C1 2.20 parts by mass ・Compound D1 0.48 parts by mass ・Compound D2 1.15 parts by mass ・Butyl acetate 100.00 parts by mass ――――――――――――――――――――――――――――――――

[0239] (Synthesis of Polymer A2) 100 parts by mass of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 500 parts by mass of methyl isobutyl ketone, and 10 parts by mass of triethylamine were charged into a reaction vessel equipped with a stirrer, thermometer, dropping funnel, and reflux condenser, and mixed at room temperature. Next, 100 parts by mass of deionized water was added dropwise from the dropping funnel over 30 minutes, and the mixture was allowed to react at 80 ° C. for 6 hours while mixing under reflux. After completion of the reaction, the organic phase was removed and washed with a 0.2% by mass aqueous ammonium nitrate solution until the water after washing became neutral. The solvent and water were then distilled off under reduced pressure to obtain an epoxy-containing polyorganosiloxane as a viscous, transparent liquid. When this epoxy-containing polyorganosiloxane was subjected to 1H-NMR (Nuclear Magnetic Resonance) analysis, a peak due to oxiranyl groups was obtained at a chemical shift (δ) of approximately 3.2 ppm, confirming the theoretical intensity and the absence of side reactions of the epoxy groups during the reaction. The weight-average molecular weight Mw of this epoxy-containing polyorganosiloxane was 2,200, and the epoxy equivalent was 186 g / mol. Next, a 100 mL three-neck flask was charged with 10.1 parts by mass of the epoxy-containing polyorganosiloxane obtained above, 0.5 parts by mass of an acrylic group-containing carboxylic acid (manufactured by Toagosei Co., Ltd., Aronix M-5300, acrylic acid ω-carboxypolycaprolactone (degree of polymerization n ≒ 2)), 20 parts by mass of butyl acetate, 1.5 parts by mass of a cinnamic acid derivative obtained by the method of Synthesis Example 1 of JP 2015-26050 A, and 0.3 parts by mass of tetrabutylammonium bromide, and stirred at 90 ° C. for 12 hours. After completion of the reaction, the reaction solution was diluted with an equal amount (by mass) of butyl acetate and washed three times with water. This solution was concentrated and the dilution with butyl acetate was repeated twice, and finally, a solution containing a polyorganosiloxane having a photoalignable group (polymer A2 below) was obtained. The weight average molecular weight Mw of this polymer A2 was 9,000. Furthermore, as a result of 1H-NMR analysis, the content of components having cinnamate groups in polymer A2 was 23.7% by mass.

[0240] Polymer A2

[0241] Low molecular weight compound B2 (Nisshin Orio Co., Ltd., Nomcoat TAB)

[0242] Crosslinking agent C1 (Crosslinking agent C1 represented by the following formula (Denacol EX411, manufactured by Nagase ChemteX Corporation))

[0243] Compound D1 (Compound D1 represented by the following formula (Kawaken Fine Chemicals Co., Ltd., Aluminum Chelate A(W)))

[0244] Compound D2 (Compound D2 represented by the following formula (manufactured by Toyo Science Co., Ltd., triphenylsilanol))

[0245] (Exposure of Alignment Film P-10) The resulting alignment film P-10 was irradiated with polarized ultraviolet light (20 mJ / cm 2 The alignment film P-10 was exposed to light by a high-pressure mercury lamp (using an ultra-high pressure mercury lamp).

[0246] <Preparation of Optically Anisotropic Layer (λ / 4 Plate)> Composition C-1 was applied onto alignment film P-10, and the coating film was heated to 110° C. on a hot plate and then cooled to 60° C. After cooling, ultraviolet light having a wavelength of 365 nm was irradiated at 500 mJ / cm using a high-pressure mercury lamp in a nitrogen atmosphere. 2 The coating film was irradiated with light at an irradiation dose of 2000 nm to fix the alignment of the liquid crystal compound, thereby producing an optically anisotropic layer. 530 ×d(Re(530)) was 132.5 nm.

[0247] ------------------------------------------------------------------ Coating liquid for forming λ / 4 plate -------------------------------------------------- Liquid crystal compound L-2 4.35 parts by mass Liquid crystal compound L-3 0.80 parts by mass Liquid crystal compound L-4 2.20 parts by mass Polymerization initiator PI-1 0.48 parts by mass Leveling agent G-1 1.15 parts by mass Methyl ethyl ketone 176.00 parts by mass Cyclopentanone 44.00 parts by mass ------------------------------------------------------------------

[0248] Liquid crystal compound L-2

[0249] Liquid crystal compound L-3

[0250] Liquid crystal compound L-4

[0251] Polymerization initiator PI-1

[0252] Leveling agent G-1

[0253] <Preparation of Circularly Polarizing Plate G> A linearly polarizing plate was attached to the support side of the optically anisotropic layer (λ / 4 plate) via an adhesive to obtain a circularly polarizing plate G.

[0254] <Preparation of Circularly Polarizing Plate B and Circularly Polarizing Plate R> In the preparation of the circularly polarizing plate G, the thickness of the optically anisotropic layer was adjusted to obtain the Δn 450 Circular polarizer B was obtained in the same manner as circular polarizer G, except that ×d(Re(450)) was set to 112.5 nm. In the production of circular polarizer G, the thickness of the optically anisotropic layer was adjusted, and the Δn 635 A circularly polarizing plate R was obtained in the same manner as for the circularly polarizing plate G, except that ×d(Re(635)) was set to 158.8 nm.

[0255] <Evaluation of Wavelength Selectivity> The polarization conversion rates of red light, green light, and blue light were evaluated when light was incident on each of the prepared optical films from the front (at an angle of 0° relative to the normal) and at a polar angle of 30° (at an angle of 30° relative to the normal). Specifically, two circular polarizers R were first arranged so that the optically anisotropic layer sides of the circular polarizers R faced each other. An optical film was also arranged between the two circular polarizers R. In this arrangement, laser light having a center wavelength of red light (635 nm) was incident on the circular polarizer R from the normal direction and converted into circularly polarized light. The circularly polarized light was then incident on the optical film from the normal direction, and the circularly polarized light emitted from the optical film was incident on the circular polarizer R, and the intensity of the red light emitted from the circular polarizer R was measured. That is, the transmittance (T R ) was measured. The incidence of the laser light was adjusted so that the direction of the transmission axis of the linear polarizer of the circular polarizer R on the side where the laser light first entered was parallel to the direction of the polarization direction of the laser light. When the above operation was performed, if the optical film generates a phase difference of λ / 2 with respect to the circularly polarized red light (converting the circularly polarized light into circularly polarized light with the opposite rotation direction), the red light is absorbed by the linear polarizer of the circular polarizer R on the side opposite to the side where the laser light entered. On the other hand, if the optical film does not generate a phase difference with respect to the circularly polarized red light (does not change the rotation direction of the circularly polarized light), the red light is not absorbed by the linear polarizer of the circular polarizer R on the side opposite to the side where the laser light entered, and the red light is emitted.

[0256] The transmittance (T) of the green laser was measured in the same manner as above, except that a circular polarizer G and a laser beam having a central output wavelength of green light (530 nm) were used. G In addition, the transmittance (T) of a blue laser was measured in the same manner as above, except that circularly polarizing plate B and a laser beam having a central output wavelength of green light (450 nm) were used. B ) was measured. R , T G , and T BThe transmittance value showing the smallest value among the above was designated T1, and the remaining values ​​were designated T2 and T3. The wavelength selectivity of the optical film was evaluated based on the following criteria. A rating is preferred because it has better wavelength selectivity. A: T1 is 30% or less, and T2 and T3 are 80% or more. B: T1 is 50% or less, and T2 and T3 are 80% or more. Note that T2 and T3 being low relative to T1 indicates that the optical film can convert only circularly polarized light in a specific wavelength range into circularly polarized light with the opposite rotation direction. This also indicates that the optical film converts circularly polarized light into circularly polarized light with the opposite rotation direction at the measurement wavelength showing T1. Furthermore, the orientation of only the optical film placed between each circular polarizer was changed so that circularly polarized light was incident from a direction tilted 30° from the normal direction to the surface of the optical film, and the same evaluation as above was performed. The evaluation results are shown in Table 5 below.

[0257]

[0258] From the results shown in Table 5, it was confirmed that the optical film (optical element) of each example can convert only circularly polarized light in a specific wavelength range into circularly polarized light in the opposite rotation direction. G is T1 (minimum transmittance), and in Example 2, T R becomes T1, and in Example 3, T B A comparison of Example 4 with the other Examples confirmed that when either a rod-shaped liquid crystal compound or a discotic liquid crystal compound was contained in the liquid crystal compound in the first liquid crystal layer and the other was contained in the liquid crystal compound in the second liquid crystal layer, excellent wavelength selectivity was achieved even when circularly polarized light was incident from a direction tilted from the normal direction to the surface of the optical film (optical element).

[0259] <Optical Elements> A first optically anisotropic member, a second optically anisotropic member, and a third optically anisotropic member were prepared by the following procedure.

[0260] [Formation of First Optically Anisotropic Member] (Support) A glass substrate was prepared as the support.

[0261] (Formation of Orientation Film) The following coating solution for forming an alignment film was applied to a support by spin coating. The support on which the coating film of the coating solution for forming an alignment film had been formed was dried on a hot plate at 60° C. for 60 seconds to form an alignment film.

[0262] Coating liquid for forming alignment film ----------------------------------- Photoalignment material A 1.00 parts by mass Water 16.00 parts by mass Butoxyethanol 42.00 parts by mass Propylene glycol monomethyl ether 42.00 parts by mass ---------------------------------------------------

[0263] -Photo alignment material A-

[0264] (Exposure of Alignment Film) The alignment film was exposed using the exposure device shown in Figure 18 to form an alignment film PG-1 having an alignment pattern. In the exposure device, a laser emitting laser light with a wavelength of 355 nm was used. The exposure amount by the interference light was 1000 mJ / cm 2 It was decided.

[0265] (Formation of Optically Anisotropic Layer) The following composition E-1 was prepared as a liquid crystal composition for forming the first optically anisotropic layer.

[0266] Composition E-1 --------------------------------------------------- Liquid crystal compound L-1 above: 10.00 parts by mass Liquid crystal compound L-5 below: 90.00 parts by mass Chiral agent C1: 0.69 parts by mass Polymerization initiator (Irgacure OXE01, manufactured by BASF): 1.00 part by mass Surfactant F2 above: 0.30 parts by mass Methyl ethyl ketone: 550.00 parts by mass Cyclopentanone: 550.00 parts by mass

[0267] Liquid crystal compound L-5

[0268] Chiral agent C1

[0269] The optically anisotropic layer was formed by applying composition E-1 in multiple layers onto the alignment film PG-1. Multilayer application refers to the process of first applying composition E-1 as a first layer onto the alignment film, heating it, and then curing it with UV light to form a liquid crystal fixation layer, and then repeatedly applying layers from the second layer onwards onto the liquid crystal fixation layer, and similarly heating it and curing it with UV light. By forming the optically anisotropic layer by multilayer application, the alignment direction of the alignment film is reflected from the bottom surface to the top surface of the optically anisotropic layer, even if the total thickness of the optically anisotropic layer is large.

[0270] First, the first layer was formed by applying the above composition E-1 onto the alignment film PG-1, heating the coating to 80°C on a hot plate, and then irradiating ultraviolet light of 365 nm wavelength at 300 mJ / cm using a high-pressure mercury lamp in a nitrogen atmosphere. 2 The coating film was irradiated with an irradiation amount of 1000 ppm, thereby fixing the orientation of the liquid crystal compound and forming a liquid crystal fixing layer.

[0271] The second and subsequent layers were coated on top of the liquid crystal fixing layer, and then heated and cured with ultraviolet light under the same conditions as above to form a liquid crystal fixing layer. In this way, coating was repeated until the desired total thickness was reached, forming an optically anisotropic layer and producing a liquid crystal diffraction element.

[0272] The complex refractive index Δn of the cured layer of liquid crystal composition E-1 was determined by measuring the retardation value and film thickness of the liquid crystal fixed layer (cured layer) obtained by applying liquid crystal composition E-1 to a separately prepared support with an alignment film for retardation measurement, aligning the director of the liquid crystal compound horizontally to the substrate, and then irradiating the layer with ultraviolet light to fix the layer. Δn can be calculated by dividing the retardation value by the film thickness. The retardation value was measured at the desired wavelength using an Axoscan manufactured by Axometrix, and the film thickness was measured using a scanning electron microscope.

[0273] The optically anisotropic layer is finally formed by 550It was confirmed by a polarizing microscope that the thickness (Re(550)) was 150 nm and that a periodic alignment surface was formed. In the liquid crystal alignment pattern of this optically anisotropic layer, one period in which the optical axis of the liquid crystal compound rotated by 180° was 0.8 μm. In addition, in this optically anisotropic layer, the twist angle of the liquid crystal compound in the thickness direction was 83°. Hereinafter, unless otherwise specified, "Δn 550 Measurements such as "×d" were carried out in the same manner.

[0274] As a liquid crystal composition for forming the second optically anisotropic layer, the following composition E-2 was prepared.

[0275] Composition E-2 ------------------------------------------------------------------- Liquid crystal compound L-1 10.00 parts by mass Liquid crystal compound L-5 90.00 parts by mass Chiral agent C1 0.03 parts by mass Polymerization initiator (Irgacure OXE01, manufactured by BASF) 1.00 part by mass Surfactant F2 0.30 parts by mass Methyl ethyl ketone 550.00 parts by mass Cyclopentanone 550.00 parts by mass

[0276] A second optically anisotropic layer was formed in the same manner as the first optically anisotropic layer, except that composition E-2 was used and the thickness of the optically anisotropic layer was adjusted.

[0277] The optically anisotropic layer is finally formed by 550 It was confirmed by a polarizing microscope that the thickness (Re(550)) of the liquid crystal layer was 335 nm and that a periodic alignment surface was formed. In the liquid crystal alignment pattern of this optically anisotropic layer, one period in which the optical axis of the liquid crystal compound rotated by 180° was 0.8 μm. In addition, in this optically anisotropic layer, the twist angle of the liquid crystal compound in the thickness direction was 8°.

[0278] As a liquid crystal composition for forming the third optically anisotropic layer, the following composition E-3 was prepared.

[0279] Composition E-3 --------------------------------------------------- Liquid crystal compound L-1 10.00 parts by mass Liquid crystal compound L-5 90.00 parts by mass Chiral agent C2 below 0.60 parts by mass Polymerization initiator (Irgacure OXE01, manufactured by BASF) 1.00 part by mass Surfactant F2 above 0.30 parts by mass Methyl ethyl ketone 550.00 parts by mass Cyclopentanone 550.00 parts by mass

[0280] A third optically anisotropic layer was formed in the same manner as the first optically anisotropic layer, except that composition E-3 was used and the thickness of the optically anisotropic layer was adjusted.

[0281] The optically anisotropic layer is finally formed by 550 It was confirmed using a polarizing microscope that the thickness (Re(550)) was 170 nm and that a periodic alignment surface was formed. In the liquid crystal alignment pattern of this optically anisotropic layer, one period in which the optical axis of the liquid crystal compound rotated by 180° was 0.8 μm. In addition, in this optically anisotropic layer, the twist angle of the liquid crystal compound in the thickness direction was -78°. In this way, a first optically anisotropic member including a first liquid crystal diffraction element A1 was produced.

[0282] Chiral agent C2

[0283] [Fabrication of Second Optically Anisotropic Member] (Formation of Alignment Film) An alignment film was formed in the same manner as described above. The alignment film was exposed to light in the following manner.

[0284] (Exposure of Alignment Film) The alignment film was exposed using the exposure device shown in Figure 18 to form an alignment film PG-2 having an alignment pattern. In the exposure device, a laser emitting laser light with a wavelength of 355 nm was used. The exposure amount by the interference light was 1000 mJ / cm 2 It was decided.

[0285] A second optically anisotropic member including a second liquid crystal diffraction element A2 was produced in the same manner as the first liquid crystal diffraction element A1, except that the alignment film PG-2 was used, and each optically anisotropic layer was adjusted to have the following phase difference.

[0286] In the second liquid crystal diffraction element A2 thus fabricated, the Δn 550 × The thickness (Re(550)) is 150 nm, the twist angle of the liquid crystal compound in the thickness direction is 83°, and the Δn 550 × The thickness (Re(550)) is 335 nm, the twist angle of the liquid crystal compound in the thickness direction is 8°, and the Δn 550 The thickness (Re(550)) was 170 nm, and the twist angle of the liquid crystal compound in the thickness direction was -78°. In the liquid crystal alignment pattern of the optically anisotropic layer of this liquid crystal diffraction element, one period in which the optical axis of the liquid crystal compound rotates by 180° was 10.0 μm.

[0287] [Preparation of Third Optically Anisotropic Member] (Formation of Alignment Film) An alignment film was formed on a support in the same manner as described above. The alignment film was exposed to light in the following manner.

[0288] (Exposure of Alignment Film) The alignment film was exposed using the exposure device shown in Figure 18 to form an alignment film PG-3 having an alignment pattern. In the exposure device, a laser emitting laser light with a wavelength of 355 nm was used. The exposure amount by interference light was 1000 mJ / cm 2 It was decided.

[0289] A third optically anisotropic member including a third liquid crystal diffraction element A3 was produced in the same manner as the first liquid crystal diffraction element A1, except that the alignment film PG-3 was used, and each optically anisotropic layer was adjusted to have the following phase difference.

[0290] In the third liquid crystal diffraction element A3 thus fabricated, the Δn 550 × The thickness (Re(550)) is 150 nm, the twist angle of the liquid crystal compound in the thickness direction is 83°, and the Δn 550× The thickness (Re(550)) is 335 nm, the twist angle of the liquid crystal compound in the thickness direction is 8°, and the Δn 550 The thickness (Re(550)) was 170 nm, and the twist angle of the liquid crystal compound in the thickness direction was -78°. In the liquid crystal alignment pattern of the optically anisotropic layer of this liquid crystal diffraction element, one period in which the optical axis of the liquid crystal compound rotates by 180° was 8.9 μm.

[0291] [Preparation and evaluation of optical element] The liquid crystal diffraction element A1 (optically anisotropic layer), the optical film (optical element) of Example 2, the liquid crystal diffraction element A2 (optically anisotropic layer), the optical film (optical element) of Example 1, and the liquid crystal diffraction element A3 (optically anisotropic layer) were laminated in this order to prepare an optical element.

[0292] The angles of the transmitted diffracted light of red, green, and blue light relative to the incident light were measured for the fabricated optical element when light was incident from the front (at an angle of 0° relative to the normal). The angle of the transmitted diffracted light is the angle of the transmitted diffracted light relative to the incident light when the incident direction of the incident light is 0°. Specifically, laser light having output center wavelengths of red light (635 nm), green light (532 nm), and blue light (450 nm) was perpendicularly incident on the fabricated optical element from a position 10 cm away from the normal direction, and the transmitted diffracted light was captured on a screen placed 100 cm away to calculate the transmission angle. In this example, the design wavelength λa of the longest wavelength light was 635 nm, the design wavelength λb of the intermediate wavelength light was 532 nm, and the design wavelength λc of the shortest wavelength light was 450 nm. The laser light was perpendicularly incident on the circular polarizers B, G, and R corresponding to each wavelength, converted into circularly polarized light, and then incident on the fabricated optical element for evaluation. Average transmission angle θ of red light, green light, and blue light ave and the maximum transmission angle θ of red light, green light, and blue light. max and the minimum transmission angle θ min From this, the wavelength dependency PE [%] of the diffraction angle of the transmitted diffracted light was calculated by the following formula. The smaller the PE, the lower the wavelength dependency of the diffraction angle of the transmitted diffracted light. PE [%] = [(θ max -θ min ) / θ ave]×100 In the fabricated optical element, the calculated PE was 5% or less, and it was confirmed that the wavelength dependency of the diffraction angle of the transmitted diffracted light was low.

[0293] REFERENCE SIGNS LIST 10 Optical element 12 First optically anisotropic member 14 Second optically anisotropic member 16 Third optically anisotropic member 18G, 18R, 100 Wavelength-selective retardation plate 20 Support 24A, 24B, 24C Alignment film 26A First optically anisotropic layer 26B Second optically anisotropic layer 26C Third optically anisotropic layer 30 Liquid crystal compound 30A Optical axis 34 Optically anisotropic layer 40 Display 42 Light guide plate 60, 80 Exposure device 62, 82 Laser 64, 84 Light source 68 Beam splitter 70A, 70B, 90A, 90B Mirror 72A, 72B, 96 λ / 4 plate 86, 94 Polarizing beam splitter 92 Lens 112 First wave plate 114 Second wave plate 116 Third wave plate 210, 230 Filter 212 First λ / 4 plate 214 Second λ / 4 plate 216, 246 Liquid crystal polarization interference element 218 Liquid crystal compound (rod-shaped liquid crystal compound) 220, 232 First liquid crystal layer 224, 234 Second liquid crystal layer 226, 236 Liquid crystal layer set D1 First in-plane slow axis direction D2 Second in-plane slow axis direction D3 Third in-plane slow axis direction B R , B 2R Right-handed circularly polarized blue light G R , G 1R , G 2R , G 3R Right-handed circularly polarized green light R R , R 1R , R 3R Right-handed circularly polarized red light B 1L , B 3L Left-handed circularly polarized blue light G 1L , G 2L Left-handed circularly polarized green light R 1L , R 2L Left circularly polarized red light M Laser light MA, MB Light MP P polarized light MS S polarized light P O Linear polarized light P R Right circular polarization P L Left circularly polarized light Q1, Q2 Absolute phase E1, E2 Equiphase surface U User

Claims

1. An optical element having, in that order, a first λ / 4 plate, an optical laminate, and a second λ / 4 plate, wherein the optical laminate has two or more liquid crystal layer pairs in the thickness direction, each pair consisting of a first liquid crystal layer having a liquid crystal compound fixed therein that is twisted in the thickness direction, and a second liquid crystal layer having a liquid crystal compound fixed therein that is twisted in the thickness direction, the twist direction of the liquid crystal compound being opposite to the twist direction of the liquid crystal compound in the first liquid crystal layer, wherein in each of the liquid crystal layer pairs, the orientation direction of the liquid crystal compound on the surface of the first liquid crystal layer facing the second liquid crystal layer is parallel to the orientation direction of the liquid crystal compound on the surface of the second liquid crystal layer facing the first liquid crystal layer, and the twist angle of the liquid crystal compound in the first liquid crystal layer is equal to the twist angle of the liquid crystal compound in the second liquid crystal layer.

2. The optical element according to claim 1, wherein one of a rod-like liquid crystal compound and a discotic liquid crystal compound is contained in the liquid crystal compound in the first liquid crystal layer, and the other is contained in the liquid crystal compound in the second liquid crystal layer.

3. The optical element described in claim 1, wherein at least one of the first λ / 4 plate and the second λ / 4 plate is a laminate consisting of a liquid crystal layer A having a liquid crystal compound fixed with a twisted alignment in the thickness direction, and a liquid crystal layer B having a liquid crystal compound fixed with a twisted alignment in the thickness direction.

4. The twist angle of the liquid crystal compound in the liquid crystal layer A is 16.5 to 36.5 degrees, and the refractive index difference Δn A and the thickness d of the liquid crystal layer A A The product Δn A d A is 252 to 312 nm, the twist angle of the liquid crystal compound in the liquid crystal layer B is 68.6 to 88.6°, and the refractive index difference Δn B and the thickness d of the liquid crystal layer B B The product Δn B d B The optical element according to claim 3, wherein the wavelength is from 110 to 170 nm.

5. The optical element described in claim 3, wherein the liquid crystal layer A is disposed on the optical laminate side, and the alignment direction of the liquid crystal compound on the liquid crystal layer A side surface of the optical laminate is parallel to the alignment direction of the liquid crystal compound on the optical laminate side surface of the liquid crystal layer A.

6. The optical element according to claim 3, wherein the alignment direction of the liquid crystal compound on the surface of the liquid crystal layer A facing the liquid crystal layer B is parallel to the alignment direction of the liquid crystal compound on the surface of the liquid crystal layer B facing the liquid crystal layer A.

7. An optical element comprising: a plurality of optically anisotropic layers formed using a composition containing a liquid crystal compound, the layers having a liquid crystal orientation pattern in which the orientation of the optical axis derived from the liquid crystal compound changes while rotating continuously along at least one direction in a plane; and an optical element according to any one of claims 1 to 6, disposed between at least a pair of adjacent two optically anisotropic layers in the plurality of optically anisotropic layers; and wherein, in the liquid crystal orientation pattern of the optically anisotropic layers, when the length of a 180° rotation of the orientation of the optical axis derived from the liquid crystal compound in the one direction in which the orientation of the optical axis derived from the liquid crystal compound changes while rotating continuously is defined as one period, at least one of the optically anisotropic layers has a length of one period different from that of the other optically anisotropic layers.

Citation Information

Patent Citations

  • Broadband polarization converter based on symmetrical multilayer twisted liquid crystal and optimization method thereof

    CN113093440A

  • Low twist chiral liquid crystal polarization diffraction grating and related manufacturing method

    JP2014089476A

  • Optical element and lightguide element

    WO2019131918A1

  • Transmissive liquid crystal diffractive element

    WO2021235416A1

Cited By

  • Laminate

    WO2026141505A1