Window film
The window film configuration addresses curling issues by using hollow silica particles and infrared-shielding metal oxides to achieve high visibility and heat shielding, enhancing workability on vehicle windows with curved surfaces.
Patent Information
- Application Number
- PCT/JP2024/010690
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-19
- Publication Date
- 2024-10-03
AI Technical Summary
Window films used for vehicle windows face challenges with curling due to curing shrinkage, which complicates installation and reduces workability, especially on large, curved surfaces, while requiring high visible light transmittance and heat ray shielding performance.
A window film configuration with a low refractive index layer formed from hollow silica particles and an active energy ray-curable component, a heat ray shielding layer made from infrared-shielding metal oxide and an active energy ray-curable component, and a hard coat layer, laminated in a specific order to suppress curling and enhance visibility and heat shielding.
The configuration achieves high visible light transmittance, effective heat ray shielding, and improved workability by balancing curing shrinkage across layers, preventing curling and ensuring smooth installation on curved surfaces.
Smart Images

Figure JP2024010690_03102024_PF_FP_ABST
Abstract
Description
window film
[0001] The present invention relates to window films.
[0002] In recent years, window films that are attached to windows of buildings and vehicles have been widely used. Such window films have an infrared shielding ability to, for example, suppress the penetration of infrared rays and prevent excessive increases in the temperature inside buildings and vehicles, thereby reducing the use of air conditioners and achieving energy savings.
[0003] On the other hand, window films used in vehicle windows, particularly windshields and front side windows, are required to have high visibility, and therefore are required to have high visible light transmittance.
[0004] Patent Document 1 discloses that in a heat-shielding window film including a metal particle-containing layer that reflects heat rays, providing a low-refractive index layer having a specific refractive index range on the outermost surface on the indoor side when the window film is installed on a window glass reduces the refractive index difference at the interface between air and the film, thereby reducing light reflection. Patent Document 1 also discloses that the low-refractive index layer preferably has hard-coating properties. Patent Document 1 also discloses that a hard-coating layer that can contain a heat-ray absorbing agent may be provided between the low-refractive index layer and the substrate.
[0005] JP 2015-118281 A
[0006] As described in Patent Document 1, when the outermost low-refractive index layer has hard coating properties, or when the film has a heat-shielding hard coating layer between the substrate and the low-refractive index layer, the window film may curl with the low-refractive index layer side facing inward. When the film curls, it becomes difficult to apply the window film to the window, resulting in a problem of reduced work efficiency. This problem is particularly serious for window films used on the front and front sides of vehicles, which have a large area and curved glass surfaces, making application difficult.
[0007] Therefore, an object of the present invention is to provide a window film that has high visible light transmittance and heat ray shielding rate, and also has improved workability.
[0008] In order to achieve at least one of the above objects, a window film according to one aspect of the present invention has the following configuration.
[0009] (1) A window film comprising a low refractive index layer, a hard coat layer, a substrate, a heat ray shielding layer, and a pressure-sensitive adhesive layer laminated in this order, wherein the low refractive index layer is formed from a composition for forming a low refractive index layer, which contains hollow silica particles and an active energy ray-curable component, and the heat ray shielding layer is formed from a composition for forming a heat ray shielding layer, which contains an infrared-shielding metal oxide and an active energy ray-curable component.
[0010] (2) The window film according to (1), wherein the thickness of the substrate is 100 μm or less.
[0011] (3) The window film according to (1) or (2), wherein the low refractive index layer is the outermost layer.
[0012] (4) The window film according to any one of (1) to (3), wherein the infrared-shielding metal oxide is at least one selected from the group consisting of indium-doped tin oxide, antimony-doped tin oxide, and cesium-doped tungsten oxide.
[0013] (5) The window film according to any one of (1) to (4), wherein the hard coat layer and the heat ray shielding layer are disposed adjacent to the substrate.
[0014] (6) The window film according to any one of (1) to (5), wherein the low refractive index layer and the hard coat layer are disposed adjacent to each other.
[0015] 1 is a cross-sectional view of a window film according to one embodiment of the present invention.
[0016] The present invention provides a window film comprising a low refractive index layer, a hard coat layer, a substrate, a heat ray shielding layer, and a pressure-sensitive adhesive layer laminated in this order, wherein the low refractive index layer is formed from a composition for forming a low refractive index layer containing hollow silica particles and an active energy ray-curable component, and the heat ray shielding layer is formed from a composition for forming a heat ray shielding layer containing an infrared-shielding metal oxide and an active energy ray-curable component.The window film of the present invention can provide a window film with high visible light transmittance and heat ray shielding rate, and also improved workability.
[0017] Window films (hereinafter simply referred to as films) are often applied using a water-based application method. Water-based application involves spraying an application liquid (e.g., a surfactant aqueous solution) onto the adhesive layer surface of the film and / or the surface of the window glass, temporarily applying the window film to the window glass, and then rubbing the film surface evenly with a spatula called a squeegee to press and remove the application liquid while adhering the film to the window glass, thereby developing adhesiveness as the water evaporates. To prevent scratches caused by squeegeeing, the film surface may be provided with a hard coat. The present inventors have found that when a hard-coated low-refractive index layer is disposed on the surface, the window film curls with the low-refractive index layer facing inward (see, for example, the comparative example described below). The present inventors speculate that this may be due to curing shrinkage that occurs when the low-refractive index layer-forming composition is applied and then cured with ultraviolet light. Based on this assumption, the inventors discovered that by forming an ultraviolet-curable heat-shielding layer that undergoes cure shrinkage on the side of the low refractive index layer opposite the substrate, curling of the window film can be suppressed and a window film with high visible light transmittance and heat-shielding rate can be obtained, thereby completing the present invention.
[0018] In this specification, the range "X to Y" means "X or more and Y or less." Unless otherwise specified, operations and measurements of physical properties are performed at room temperature (20 to 25°C) and a relative humidity of 45 to 55% RH. In this specification, "(meth)acrylic acid" refers to "acrylic acid or methacrylic acid," and "(meth)acrylate" refers to "acrylate or methacrylate."
[0019] Hereinafter, an embodiment of the present invention will be described with reference to the accompanying drawings. In the description of the drawings, the same elements are designated by the same reference numerals, and duplicate explanations will be omitted. Furthermore, the dimensional proportions in the drawings are exaggerated for the convenience of explanation and may differ from the actual proportions.
[0020] FIG. 1 is a cross-sectional view of a window film according to one embodiment of the present invention. The drawings are exaggerated for ease of explanation, and the dimensional proportions of the various components in the drawings may differ from the actual figures. In FIG. 1 , the window film 10 is composed of a low refractive index layer 11, a hard coat layer 12, a substrate 13, a heat-shielding layer 14, a pressure-sensitive adhesive layer 15, and a release liner 16. The pressure-sensitive adhesive layer 15 is disposed to bond the window film to the window glass as an adherend. The low refractive index layer 11 is the outermost layer. Because the low refractive index layer 11 contains an active energy ray-curable resin, even when disposed as the outermost layer, it can prevent scratches caused by squeegee processing, and its placement as the outermost layer can further increase visible light transmittance. Furthermore, the hard coat layer 12 and the heat-shielding layer 14 are disposed adjacent to the substrate 13. This arrangement is preferable because it ensures that both sides of the substrate experience similar cure shrinkage, thereby suppressing curling of the window film. The release liner 16 protects the pressure-sensitive adhesive layer 15 and prevents a decrease in adhesiveness. The release liner 16 is peeled off from the window film when the film is attached to the adherend. Therefore, window films that do not have a release liner 16 are also within the technical scope of the present invention. The window film may be attached to the interior (vehicle interior) side of the window glass or the exterior (vehicle exterior) side of the window glass, but in consideration of durability, it is preferably attached to the interior (vehicle interior) side of the window glass. In an embodiment in which the window film is attached to the interior (vehicle interior) side of the window glass, the pressure-sensitive adhesive layer side is the (sunlight) incident side.
[0021] In the embodiment shown in Fig. 1, the window film 10 is composed of a low refractive index layer 11, a hard coat layer 12, a substrate 13, a heat-shielding layer 14, a pressure-sensitive adhesive layer 15, and a release liner 16. However, as long as the low refractive index layer 11, the hard coat layer 12, the substrate 13, the heat-shielding layer 14, the pressure-sensitive adhesive layer 15, and the release liner 16 are arranged in this order, other functional layers (e.g., a printing layer, an antistatic layer, an adhesion-improving layer, a light-shielding layer, a stress relaxation layer, an anti-fogging layer, an anti-fouling layer, an ultraviolet-reflecting layer, etc.) may be present between the layers. Note that a preferred embodiment is one in which the low refractive index layer 11 and the hard coat layer 12 are adjacent to each other, as shown in Fig. 1. This arrangement is preferable from the viewpoints of improving visible light transmittance, ensuring scratch resistance, and reducing the thickness of the film.
[0022] The components of the window film of the present invention will be described below.
[0023] (Low refractive index layer) The low refractive index layer is formed from a composition for forming a low refractive index layer containing hollow silica particles and an active energy ray-curable component. The inclusion of hollow silica particles allows the layer to exhibit anti-reflection properties due to the difference in refractive index between air and the particles.
[0024] Hollow silica particles have fine voids within the particles, either open or closed. Because the voids of hollow silica particles are filled with gas (air), they have a relatively low refractive index, reducing light reflection. The shape of the hollow silica particles is not particularly limited, but spherical, spindle-shaped, oval, tabular, cubic, and amorphous shapes are preferred. Of these, spherical, tabular, and cubic shapes are particularly preferred. The hollow silica particles may have closed cells, open cells, or both closed and open cells. The hollow silica particles may be modified with an organic substance to improve dispersibility. The hollow silica particles are also preferably in the form of an organosol (colloidal) (hollow silica sol).
[0025] In the hollow silica particles, the proportion of voids is preferably 5% or more, more preferably 10 to 80%, and even more preferably 20 to 60% of the volume.
[0026] The average particle size of the hollow silica particles is preferably 5 nm or more and 100 nm or less, more preferably 20 nm or more and 80 nm or less, and even more preferably 40 nm or more and 70 nm or less. When the average particle size of the hollow silica particles is within these preferred ranges, the low refractive index layer can achieve excellent anti-reflection effect and transparency. The average particle size is a volume-based average arithmetic value obtained by a laser diffraction / scattering method.
[0027] The refractive index of the hollow silica particles is preferably in the range of 1.01 to 1.45, more preferably in the range of 1.15 to 1.38, and even more preferably in the range of 1.15 to 1.35. Within this range, excellent anti-reflection effects can be obtained. Note that the refractive index of the hollow silica particles in this specification is measured by the minimum deviation angle method.
[0028] The content of hollow silica particles in the low refractive index layer is preferably 20 to 80% by mass, and more preferably 30 to 60% by mass, from the viewpoint of excellent antireflection effect.
[0029] Examples of the active energy ray-curable component include a polyfunctional (meth)acrylate monomer, a (meth)acrylate prepolymer, and an active energy ray-curable polymer. These may be used alone or in combination of two or more. Among these, the active energy ray-curable component used in the composition for forming a low refractive index layer is preferably a polyfunctional (meth)acrylate monomer and / or a (meth)acrylate prepolymer.
[0030] Examples of polyfunctional (meth)acrylate monomers include bifunctional monomers such as 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, neopentyl glycol adipate di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, caprolactone-modified dicyclopentenyl di(meth)acrylate, ethylene oxide-modified phosphate di(meth)acrylate, di(acryloxyethyl)isocyanurate, allylated cyclohexyl di(meth)acrylate, ethoxylated bisphenol A diacrylate, and 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene; Examples of such trifunctional acrylates include methylolpropane tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, propionic acid-modified dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide-modified trimethylolpropane tri(meth)acrylate, tris(acryloxyethyl)isocyanurate, and ε-caprolactone-modified tris-(2-(meth)acryloxyethyl)isocyanurate; tetrafunctional acrylates such as diglycerin tetra(meth)acrylate and pentaerythritol tetra(meth)acrylate; pentafunctional acrylates such as propionic acid-modified dipentaerythritol penta(meth)acrylate; and hexafunctional acrylates such as dipentaerythritol hexa(meth)acrylate and caprolactone-modified dipentaerythritol hexa(meth)acrylate. These acrylates may be used alone or in combination of two or more. Among these, from the viewpoint of the hardness of the low refractive index layer to be formed, the polyfunctional (meth)acrylate monomer is preferably trifunctional or more, and more preferably tetrafunctional or more.
[0031] Examples of (meth)acrylate-based prepolymers include polyester (meth)acrylate-based, epoxy (meth)acrylate-based, urethane (meth)acrylate-based, polyol (meth)acrylate-based prepolymers, etc. Among these, in terms of the hardness of the low refractive index layer to be formed and the ability to be applied to curved surfaces, urethane (meth)acrylate-based prepolymers are preferred as the (meth)acrylate-based prepolymers.
[0032] The polyester (meth)acrylate prepolymer can be obtained, for example, by esterifying the hydroxyl groups of a polyester oligomer having hydroxyl groups at both ends, obtained by condensation of a polycarboxylic acid and a polyhydric alcohol, with (meth)acrylic acid, or by esterifying the terminal hydroxyl groups of an oligomer obtained by adding an alkylene oxide to a polycarboxylic acid, with (meth)acrylic acid.
[0033] The epoxy (meth)acrylate prepolymer can be obtained, for example, by reacting (meth)acrylic acid with the oxirane ring of a relatively low molecular weight bisphenol epoxy resin or novolac epoxy resin to esterify it.
[0034] The urethane (meth)acrylate prepolymer can be obtained, for example, by esterifying a polyurethane oligomer obtained by reacting a polyether polyol or polyester polyol with a polyisocyanate with (meth)acrylic acid.
[0035] The polyol acrylate prepolymer can be obtained, for example, by esterifying the hydroxyl groups of a polyether polyol with (meth)acrylic acid.
[0036] The prepolymers may be used singly or in combination of two or more.
[0037] The content of the active energy ray curable component in the composition for forming a low refractive index layer is preferably 20 to 80 mass %, more preferably 40 to 70 mass %, in terms of solid content, in consideration of hard coat properties.
[0038] The composition for forming a low refractive index layer may contain various additives in addition to the above components. Examples of the various additives include photopolymerization initiators, surface conditioners, leveling agents, antifouling agents, dispersants, ultraviolet absorbers, antioxidants, light stabilizers, antistatic agents, silane coupling agents, antiaging agents, thermal polymerization inhibitors, colorants, refractive index adjusters, surfactants, storage stabilizers, plasticizers, lubricants, antifoaming agents, organic fillers, wettability improvers, and coating surface improvers. The composition for forming a low refractive index layer may or may not contain the following infrared-shielding metal oxides. Specifically, the composition for forming a low refractive index layer may or may not contain zinc oxide, tungsten oxide, antimony-doped zinc oxide (AZO), indium-doped zinc oxide (IZO), gallium-doped zinc oxide (GZO), aluminum-doped zinc oxide, tin oxide, antimony-doped tin oxide (ATO), indium-doped tin oxide (ITO), cesium-doped tungsten oxide (CWO (registered trademark)), etc. In one embodiment, the composition for forming a low refractive index layer preferably does not substantially contain the following infrared-shielding metal oxides. Specifically, the composition for forming a low refractive index layer preferably does not substantially contain any of zinc oxide, tungsten oxide, antimony-doped zinc oxide (AZO), indium-doped zinc oxide (IZO), gallium-doped zinc oxide (GZO), aluminum-doped zinc oxide, tin oxide, antimony-doped tin oxide (ATO), indium-doped tin oxide (ITO), and cesium-doped tungsten oxide (CWO (registered trademark)). Here, "substantially free" means that the content in the layer is 0.1% by mass or less (lower limit: 0% by mass), preferably 0.01% by mass or less (lower limit: 0% by mass), and more preferably 0.001% by mass or less (lower limit: 0% by mass).
[0039] Examples of the photopolymerization initiator include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin-n-butyl ether, benzoin isobutyl ether, acetophenone, dimethylaminoacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one, 4-(2-hydroxyphenyl)-2 ... Examples of the hydroxybenzoates include (hydroxyethoxy)phenyl-2-(hydroxy-2-propyl)ketone, benzophenone, p-phenylbenzophenone, 4,4'-diethylaminobenzophenone, dichlorobenzophenone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 2-aminoanthraquinone, 2-methylthioxanthone, 2-ethylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, benzyl dimethyl ketal, acetophenone dimethyl ketal, and p-dimethylaminobenzoic acid esters. These may be used alone or in combination of two or more.
[0040] The content of the photopolymerization initiator in the composition for forming a low refractive index layer is preferably 0.01 to 20 parts by mass, and more preferably 0.1 to 15 parts by mass, relative to 100 parts by mass of the active energy ray-curable component.
[0041] Considering the refractive index, the thickness of the low refractive index layer is preferably 20 to 300 nm, more preferably 40 to 200 nm, and even more preferably 60 to 150 nm.
[0042] When the low refractive index layer is disposed as the outermost layer, the pencil hardness of the low refractive index surface of the window film is preferably F or higher, more preferably H or higher, and even more preferably 2H or higher. When the low refractive index layer has such a pencil hardness, the surface of the window film has sufficient hardness and can exhibit excellent scratch resistance. The upper limit of the pencil hardness is not particularly limited, but is preferably 9H or lower. The pencil hardness is measured using an electric pencil scratch hardness tester (manufactured by Yasuda Seiki Seisakusho, product name "No. 553-M1") in accordance with JIS K5600-5-4:1999.
[0043] (Hard Coat Layer) The hard coat layer is provided to improve scratch resistance. Since the low refractive index layer has a thin thickness of typically on the order of nanometers by controlling the refractive index, scratch resistance can be ensured by further providing a hard coat layer.
[0044] The hard coat layer is, for example, a cured product of a hard coat agent (a composition for forming a hard coat layer). The hard coat agent usually contains an active energy ray-curable component.
[0045] Examples of active energy ray-curable components include polyfunctional (meth)acrylate monomers, (meth)acrylate prepolymers, and active energy ray-curable polymers. These may be used alone or in combination. Among these, polyfunctional (meth)acrylate monomers and / or (meth)acrylate prepolymers are preferred as the active energy ray-curable components used in the hard coat layer-forming composition. The polyfunctional (meth)acrylate monomers and (meth)acrylate prepolymers may be used alone or in combination. Specific examples and preferred embodiments of these are the same as those described in the section on the low refractive index layer above. Furthermore, the active energy ray-curable component used in the hard coat layer-forming composition may be the same material as or different from the active energy ray-curable component used in the low refractive index layer-forming composition.
[0046] The content of the active energy ray-curable component in the hard coating agent is preferably 70 to 100 mass %, more preferably 75 to 99 mass %, in terms of solid content, in consideration of hard coating properties.
[0047] In addition to the above components, the hard coat layer may contain various additives. Examples of the various additives include photopolymerization initiators, stabilizers, surfactants, ultraviolet absorbers, flame retardants, antistatic agents, antioxidants, heat stabilizers, lubricants, fillers, colorants, pigments, and adhesion modifiers. In the present invention, since the heat-shielding layer is present, the hard coat layer does not necessarily require an infrared-shielding agent such as an infrared-shielding metal oxide or an infrared absorber. The hard coat layer may or may not substantially contain an infrared-shielding agent. Specifically, the hard coat layer-forming composition may or may not contain zinc oxide, tungsten oxide, antimony-doped zinc oxide (AZO), indium-doped zinc oxide (IZO), gallium-doped zinc oxide (GZO), aluminum-doped zinc oxide, tin oxide, antimony-doped tin oxide (ATO), indium-doped tin oxide (ITO), cesium-doped tungsten oxide (CWO (registered trademark)), and the like. Here, "substantially free" means that the content in the layer is 0.1% by mass or less (lower limit: 0% by mass), preferably 0.01% by mass or less (lower limit: 0% by mass), and more preferably 0.001% by mass or less (lower limit: 0% by mass).
[0048] Specific examples of the photopolymerization initiator that can be used in the hard coating agent include those described above in the section on the low refractive index layer.
[0049] The content of the photopolymerization initiator in the hard coating agent is preferably 0.01 to 20 parts by mass, and more preferably 0.1 to 15 parts by mass, relative to 100 parts by mass of the active energy ray-curable component.
[0050] From the viewpoint of scratch resistance and film hardness, the thickness of the hard coat layer is preferably 0.1 to 20 μm, more preferably 0.5 to 10 μm, and even more preferably 1 to 5 μm.
[0051] The pencil hardness of the hard coat layer is preferably F or more, more preferably H or more, and even more preferably 2H or more. When the hard coat layer has such a pencil hardness, it is possible to achieve a balance in hardness with the low refractive index layer and the laminate of the hard coat layer, which is effective in suppressing curling. The pencil hardness of the hard coat layer can be determined by exposing the hard coat layer and measuring the pencil hardness of the hard coat layer surface.
[0052] (Substrate) The material for forming the substrate is not particularly limited, but is preferably a resin substrate. The substrate may be a single layer or a laminated film of two or more layers.
[0053] The resin substrate may be a stretched film such as a uniaxially stretched film or a biaxially stretched film, or may be a non-stretched film, or may be formed by a casting method or the like using a processing material.
[0054] From the viewpoint of visibility, the substrate is preferably transparent. Here, "transparent" means that the total light transmittance is 80% or more, preferably 90% or more (upper limit: 100%). Here, the transmittance of the substrate can be measured according to JIS K7361-1:1997 (Test method for total light transmittance of plastic transparent materials).
[0055] The material constituting the resin substrate is not particularly limited, and examples thereof include polyester-based resins such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polyolefin-based resins such as polyethylene, polypropylene, poly4-methylpentene-1, and polybutene-1; cellulose-based resins such as cellophane, diacetyl cellulose, triacetyl cellulose, and acetyl cellulose butyrate; polyvinyl chloride-based resins; polyvinylidene chloride-based resins; polyvinyl alcohol-based resins; polystyrene-based resins; polycarbonate-based resins; polysulfone-based resins; fluorine-based resins; acrylic resins; cyclic olefin-based resins such as norbornene-based resins; polyamide resins; and styrene-based resins. These materials constituting the resin substrate may be used alone or in combination of two or more. Among these, from the viewpoint of transparency, polyester-based resins and polyolefin-based resins are preferred as the material constituting the resin substrate, with polyethylene terephthalate, polyethylene, and polypropylene being more preferred, and polyethylene terephthalate being even more preferred.
[0056] The substrate may be in a form in which a primer layer is provided on a resin substrate. The primer layer may be formed on one side or both sides of the resin substrate. As the primer layer, for example, an acrylic-based, polyester-based, polyurethane-based, rubber-based, or other primer layer can be used as appropriate. The thickness of the primer layer may be, for example, 0.1 to 10 μm, or may be, for example, 0.5 to 5 μm.
[0057] The substrate may contain, as needed, stabilizers, lubricants, fillers, colorants, processing aids, softeners, metal powders, anti-fogging agents, ultraviolet absorbers, antioxidants, antistatic agents, flame retardants, and the like.
[0058] The thickness of the substrate is, for example, 5 to 150 μm. The thickness of the substrate is preferably 100 μm or less, since it is easy to follow the curved surface of the adherend, i.e., window glass (curved surface conformability). A thinner substrate is preferable in terms of curved surface conformability, but the thinner the substrate, the more serious the curl problem becomes. However, according to this embodiment, even if the substrate is thin, for example, 100 μm or less, curl can be sufficiently suppressed. The thickness of the substrate is preferably 10 to 100 μm, more preferably 10 to 50 μm, and even more preferably 10 to 30 μm.
[0059] (Heat-ray shielding layer) The heat-ray shielding layer contains an infrared-shielding metal oxide and an active energy ray-curable component.
[0060] The infrared-shielding metal oxide is preferably infrared-absorbing in terms of visible light transmittance. Specific examples of infrared-absorbing metal oxides include zinc oxide, tungsten oxide, antimony-doped zinc oxide (AZO), indium-doped zinc oxide (IZO), gallium-doped zinc oxide (GZO), aluminum-doped zinc oxide, tin oxide, antimony-doped tin oxide (ATO), indium-doped tin oxide (ITO), and cesium-doped tungsten oxide (CWO (registered trademark)). These infrared-shielding metal compounds may be used alone or in combination of two or more. Among them, the infrared-shielding metal compound is more preferably at least one selected from the group consisting of indium-doped tin oxide (ITO), antimony-doped tin oxide (ATO), and cesium-doped tungsten oxide (CWO (registered trademark)) because of its high visible light transmittance.
[0061] The content of the infrared-shielding metal compound in the heat-ray-shielding layer is appropriately set in consideration of the heat-shielding effect and visible light transmittance. For example, the content of the infrared-shielding metal compound in the heat-ray-shielding layer is preferably 20 to 80 mass %, more preferably 40 to 75 mass %, and even more preferably 50 to 70 mass %.
[0062] The heat ray shielding layer is formed from a composition for forming a heat ray shielding layer, which contains an active energy ray curable component.
[0063] Examples of active energy ray-curable components include polyfunctional (meth)acrylate monomers, (meth)acrylate prepolymers, and active energy ray-curable polymers. These may be used alone or in combination of two or more. Among these, the active energy ray-curable component used in the heat-ray-shielding layer-forming composition is preferably a polyfunctional (meth)acrylate monomer and / or a (meth)acrylate prepolymer. The polyfunctional (meth)acrylate monomer and the (meth)acrylate prepolymer may be used alone or in combination. Specific examples and preferred embodiments of these are the same as those described above in the section on the low refractive index layer. The active energy ray-curable component used in the heat-ray-shielding layer-forming composition may be the same material as or different from the active energy ray-curable component used in the low refractive index layer-forming composition and the active energy ray-curable component used in the hard coat layer-forming composition.
[0064] The content of the active energy ray-curable component in the composition for forming a heat ray-shielding layer is preferably 20 to 80 mass %, and more preferably 30 to 50 mass %, in terms of solid content, in consideration of the balance of hardness with the low refractive index layer and the hard coat layer.
[0065] The thickness of the heat ray shielding layer is preferably 1 to 10 μm, taking into consideration the heat ray shielding effect and the balance with the low refractive index layer (curl suppression effect).
[0066] The pencil hardness of the heat-ray-shielding layer is preferably F or more, more preferably H or more, and even more preferably 2H or more. When the heat-ray-shielding layer has such a pencil hardness, it is possible to achieve a balance in hardness with the laminate of the low refractive index layer and the hard coat layer, which is effective in suppressing curling. The pencil hardness of the heat-ray-shielding layer can be determined by exposing the heat-ray-shielding layer and measuring the pencil hardness of the heat-ray-shielding layer surface.
[0067] In consideration of suppressing curling, the thickness ratio of the hard coat layer to the heat ray shielding layer is preferably 0.5 to 1.5, more preferably 0.8 to 1.2, where the thickness of the hard coat layer is the thickness of the heat ray shielding layer.
[0068] The heat-ray shielding layer may contain various additives in addition to the above components, such as a photopolymerization initiator, a stabilizer, a surfactant, an ultraviolet absorber, an antistatic agent, an antioxidant, a heat stabilizer, a lubricant, a filler, a colorant, a pigment, and an adhesion adjuster.
[0069] Specific examples of the photopolymerization initiator that can be used in the heat ray shielding layer include those described above in the section on the low refractive index layer.
[0070] The content of the photopolymerization initiator in the heat ray-shielding layer is preferably 0.01 to 20 parts by mass, more preferably 0.1 to 15 parts by mass, based on 100 parts by mass of the active energy ray-curable component.
[0071] (Adhesive Layer) The adhesive layer is used on the heat ray shielding layer side of the substrate.
[0072] The adhesive used in the adhesive layer is not particularly limited, and may be an acrylic adhesive, a rubber adhesive, a silicone adhesive, a urethane adhesive, a polyester adhesive, a styrene-diene block copolymer adhesive, a vinyl alkyl ether adhesive, a polyamide adhesive, a fluorine-based adhesive, etc. The above adhesives may be used alone or in combination of two or more.
[0073] As the adhesive, from the viewpoint of adhesive reliability, an acrylic adhesive can be particularly preferably used.
[0074] The acrylic copolymer constituting the acrylic pressure-sensitive adhesive is formed by using a (meth)acrylic acid alkyl ester as the main monomer component, and optionally a monomer copolymerizable with the (meth)acrylic acid alkyl ester (copolymerizable monomer). Here, the main component refers to 50% by mass or more (up to 100% by mass) of the monomers, and the content of the (meth)acrylic acid alkyl ester relative to the total monomers is, in order of preference, 65% by mass or more, 85% by mass or more, and 90% by mass or more.
[0075] Examples of (meth)acrylic acid alkyl esters include 2-ethylhexyl (meth)acrylate, n-butyl (meth)acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, isooctyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, myristyl (meth)acrylate, palmityl (meth)acrylate, and stearyl (meth)acrylate. These may be used alone or in combination of two or more. Among these, from the viewpoint of adhesive performance, the (meth)acrylic acid alkyl ester is preferably at least one selected from the group consisting of 2-ethylhexyl (meth)acrylate, methyl (meth)acrylate, and n-butyl (meth)acrylate, more preferably n-butyl (meth)acrylate, and even more preferably n-butyl acrylate.
[0076] When a crosslinking agent is used, it is preferable to further use a vinyl monomer containing a functional group capable of reacting with the crosslinking agent (hereinafter also referred to as a crosslinkable functional group-containing vinyl monomer).
[0077] The functional group in the crosslinkable functional group-containing vinyl monomer varies depending on the crosslinking agent selected, but examples thereof include a carboxyl group, an acid anhydride group, a hydroxyl group, a glycidyl group, an amino group, an amide group, a nitrile group, etc. Among these, the crosslinkable functional group-containing vinyl monomer is preferably a crosslinkable functional group-containing vinyl monomer selected from at least one of a carboxyl group-containing vinyl monomer and a hydroxyl group-containing vinyl monomer, since this can ensure high cohesive strength.
[0078] The crosslinkable functional group-containing vinyl monomer may be used alone or in combination of two or more kinds.
[0079] Examples of the carboxyl group- or acid anhydride group-containing vinyl monomer include (meth)acrylic acid, maleic acid, maleic anhydride, fumaric acid, crotonic acid, itaconic acid, itaconic anhydride, myristoleic acid, palmitoleic acid, and oleic acid. Among these, (meth)acrylic acid is preferred from the viewpoint of polymerizability.
[0080] The hydroxyl group-containing vinyl monomer is not particularly limited as long as it has a polymerizable functional group with an unsaturated double bond, such as a (meth)acryloyl group or a vinyl group, and also has a hydroxyl group. From the viewpoint of copolymerizability with a (meth)acrylic acid alkyl ester, the hydroxyl group-containing vinyl monomer is preferably a (meth)acrylic acid hydroxyalkyl ester. Examples of the (meth)acrylic acid hydroxyalkyl ester include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. Among these, from the viewpoint of crosslinkability, it is preferable to use at least one selected from the group consisting of 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 2-hydroxybutyl (meth)acrylate, and it is more preferable to use 2-hydroxyethyl (meth)acrylate.
[0081] The content of the crosslinkable functional group-containing vinyl monomer is preferably 0.1 to 20% by mass of the total monomers. When the content of the crosslinkable functional group-containing vinyl monomer is in this range, the crosslink density becomes appropriate and adhesiveness is maintained.
[0082] The molecular weight of the acrylic copolymer is not particularly limited, but the weight average molecular weight (Mw) is, for example, 100,000 to 2,000,000, and may be 200,000 to 1,000,000. In this specification, the weight average molecular weight (Mw) is measured by gel permeation chromatography (GPC) as a standard polystyrene equivalent molecular weight.
[0083] The method for producing the acrylic copolymer is not particularly limited, and any conventionally known method can be used, such as solution polymerization using a polymerization initiator, emulsion polymerization, suspension polymerization, reversed-phase suspension polymerization, thin-film polymerization, spray polymerization, etc. In addition to the method of initiating polymerization using a polymerization initiator, a method of initiating polymerization by irradiation with radiation, electron beams, ultraviolet rays, etc. can also be used.
[0084] The pressure-sensitive adhesive can be formed from a pressure-sensitive adhesive composition. The content (solid content) of the acrylic copolymer in the pressure-sensitive adhesive composition is preferably 50 to 100 mass %, more preferably 60 to 100 mass %.
[0085] The pressure-sensitive adhesive composition may contain a crosslinking agent in addition to the acrylic copolymer. Examples of crosslinking agents include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, and metal chelate-based crosslinking agents. The amount of crosslinking agent added is preferably 0.001 to 10 parts by mass, and more preferably 0.05 to 5 parts by mass, per 100 parts by mass of the acrylic copolymer. The crosslinking agent may be used alone or in the form of a mixture of two or more types.
[0086] The PSA composition may further contain other conventionally known additives, such as fillers, pigments, UV absorbers, tackifiers, etc. Examples of fillers include zinc oxide, silica, calcium carbonate, etc.
[0087] The thickness of the pressure-sensitive adhesive layer may usually be 5 to 100 μm, or may be 5 to 50 μm.
[0088] (Release Liner) The release liner is a component that protects the pressure-sensitive adhesive layer and prevents a decrease in adhesiveness. The release liner is peeled off from the pressure-sensitive adhesive sheet when the film is attached to an adherend. For this reason, the window film of the present invention also includes those that do not have a release liner.
[0089] The release liner is not particularly limited, but examples thereof include plastic films such as polyester films such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate, and polyolefin films such as polypropylene and polyethylene; and papers such as fine paper, glassine paper, clay-coated paper, and polyethylene-laminated paper.
[0090] The thickness of the release liner is usually about 10 to 400 μm. The surface of the release liner may be provided with a layer of a release agent made of silicone or the like to improve the releasability of the pressure-sensitive adhesive layer. When such a layer is provided, the thickness of the layer is usually about 0.01 to 5 μm.
[0091] <Manufacturing Method> In a preferred method for manufacturing the window film, for example, the hard coat layer 12 and the low refractive index layer 11 are sequentially formed on one side of the substrate 13, and then the heat ray-shielding layer 14 is formed on the side of the substrate 13 opposite to the low refractive index layer 11. Alternatively, the heat ray-shielding layer 14 is formed on one side of the substrate 13, and then the hard coat layer 12 and the low refractive index layer 11 are sequentially formed on the side of the substrate 13 opposite to the heat ray-shielding layer 14.
[0092] Specifically, for example, a hard coating agent may be applied to the substrate 13 and then cured, for example, by ultraviolet light to form the hard coating layer 12, and then a composition for forming a low refractive index layer may be applied on the hard coating layer 12 and then cured, for example, by ultraviolet light to form the low refractive index layer 11. Furthermore, for example, a composition for forming a heat ray-shielding layer may be applied to the surface of the substrate 13 opposite to the low refractive index layer 11 and then cured, for example, by ultraviolet light to form the heat ray-shielding layer 14.
[0093] The low refractive index layer-forming composition, hard coating agent, and heat ray-shielding layer-forming composition may contain a solvent if desired. Examples of the solvent include esters such as ethyl acetate and butyl acetate; ketones such as methyl isobutyl ketone, methyl ethyl ketone, and cyclohexanone; and aromatic hydrocarbons such as toluene and xylene. These solvents may be used alone or in combination of two or more.
[0094] The method for applying the composition for forming a low refractive index layer, the hard coating agent, and the composition for forming a heat ray-shielding layer is not particularly limited, and they can be applied using a known application device such as a roll coater, a knife coater, an air knife coater, a bar coater, a blade coater, a slot die coater, a lip coater, or a gravure coater.
[0095] After application, each composition may be dried. The drying conditions are not particularly limited, but may be, for example, at 80 to 120° C. for 30 seconds to 2 minutes.
[0096] Examples of ultraviolet irradiation sources include mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, xenon lamps, metal halides, LEDs, etc. The amount of ultraviolet irradiation is not particularly limited as long as a cured product is formed, but the cumulative amount of light is usually 10 to 2000 mJ / cm. 2 The range is.
[0097] The method for forming the pressure-sensitive adhesive layer is not particularly limited, and the pressure-sensitive adhesive layer may be formed by directly applying a pressure-sensitive adhesive composition onto the heat-ray-shielding layer, or the pressure-sensitive adhesive layer may be formed on a release liner, and then the release liner may be attached to the heat-ray-shielding layer surface of a laminate of low refractive index layer-hard coat layer-substrate-heat-ray-shielding layer.
[0098] The method for applying the PSA composition to the substrate or release liner is not particularly limited, and the composition can be applied using a known application device such as a roll coater, knife coater, air knife coater, bar coater, blade coater, slot die coater, lip coater, gravure coater, etc. Drying conditions are not particularly limited, and drying is usually performed at 60 to 150°C for 10 to 60 seconds.
[0099] The thickness of the pressure-sensitive adhesive layer (film thickness after drying) is usually 5 to 100 μm, preferably 10 to 50 μm.
[0100] (Visible Light Transmittance) The visible light transmittance of the window film is preferably 60% or more (upper limit 100%), more preferably 70% or more, and even more preferably 80% or more. When the visible light transmittance is equal to or greater than the lower limit, high visibility is ensured even when the film is attached to the windshield or front side window of a vehicle. The visible light transmittance is measured by the method described in the examples.
[0101] (Infrared Reflectance) From the viewpoint of heat-shielding performance, the infrared reflectance of the window film is preferably 30% or less, and more preferably 20% or less. The infrared reflectance is measured by the method described in the examples.
[0102] (Uses) The window film of the present invention can be applied to windows of buildings, vehicles (e.g., cars), etc. Examples of vehicles include cars, trains, and streetcars. When the window film is applied to an automobile window, examples of the window glass of the automobile to which it is applied include the windshield, rear windshield, front bench glass, front door glass, rear door glass, rear quarter glass, and rear side glass. Among these, because transparency is required, the windshield, front bench glass, and front door glass are preferred as the window glass of the automobile to which it is applied. In addition, suitable materials for the window include, for example, glass and glass-substitute resins. Examples of glass-substitute resins include, but are not limited to, polycarbonate resins, polysulfone resins, acrylic resins, polyolefin resins, polyether resins, polyester resins, polyamide resins, polysulfide resins, unsaturated polyester resins, epoxy resins, melamine resins, phenolic resins, diallyl phthalate resins, polyimide resins, styrene resins, and vinyl chloride resins.
[0103] The window film can be applied, for example, by so-called water application. Specifically, water application involves applying an aqueous medium to at least one of the contact surfaces of the film, contacting the pressure-sensitive adhesive layer surface with the adherend, and removing the aqueous medium as necessary. The aqueous medium is used as a so-called application liquid. An aqueous medium refers to a medium containing 50% by mass or more of water (up to 100% by mass), preferably 70% by mass or more, more preferably 85% by mass or more, and most preferably water. Furthermore, a surfactant is usually contained in the application liquid for water application to improve the sliding properties between the adherend and the film.
[0104] Next, the adhesive layer surface is brought into contact with the adherend. That is, the adhesive layer surface of the film is aligned with the adherend. At this time, the release liner is removed. The application position of the window film can be adjusted by sliding the adhesive film against the adherend via the aqueous medium (application liquid).
[0105] Thereafter, the aqueous medium is removed and the window film is applied to the adherend.
[0106] One method for removing (discharging) the aqueous medium present between the adherend and the window film is to uniformly rub the film surface with a squeegee in sequence to push out and remove the aqueous medium. In this process, air bubbles formed between the window film and the adherend can be pushed out, and wrinkles formed in the window film can be smoothed out.
[0107] The effects of the present invention will be explained using the following examples and comparative examples. In the examples, the terms "parts" and "%" are sometimes used, but unless otherwise specified, they represent "parts by mass" or "% by mass." Furthermore, unless otherwise specified, each operation is carried out at room temperature (25°C).
[0108] Example 1 1. Formation of Hard Coat Layer 100 parts by mass of a urethane acrylate prepolymer (manufactured by Arakawa Chemical Industries, Ltd., product name "BEAMSET 575CB") as an active energy ray-curable component and 3 parts by mass of 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one as a photopolymerization initiator were mixed in a 1:1 (mass ratio) mixed solvent of cyclohexanone and methyl isobutyl ketone to obtain a coating liquid of a composition for forming a hard coat layer.
[0109] The obtained coating liquid of the composition for forming a hard coat layer was applied to a transparent substrate PET film (thickness 25 μm, COSMOSHINE (registered trademark) A4360 (manufactured by Toyobo Co., Ltd.)) using a Mayer bar and dried at 90°C for 1 minute. Next, under a nitrogen atmosphere, ultraviolet light was irradiated using an ultraviolet irradiation device (manufactured by Eye Graphics Co., Ltd., product name "Eigrantage ECS-401GX type") under the following conditions to form a hard coat layer with a thickness of 3 μm. [Ultraviolet light irradiation conditions] Light source: high-pressure mercury lamp Lamp power: 2 kW Conveyor speed: 4.23 m / min Illuminance: 300 mW / cm 2 ・Light intensity: 250mJ / cm 2
[0110] 2. Formation of Low Refractive Index Layer 100 parts by mass of a urethane acrylate prepolymer (manufactured by Arakawa Chemical Industries, Ltd., product name "Beamset 575CB") as an active energy ray-curable component, 100 parts by mass (solids content) of a silica sol containing hollow silica particles (manufactured by JGC Catalysts and Chemicals, product name "Surulia 4320", solids content 20.5%, solvent: methyl isobutyl ketone, average particle size of hollow silica particles: 60 nm, refractive index 1.25), and 3 parts by mass of 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one as a photopolymerization initiator were mixed in a 1:1 (mass ratio) mixed solvent of cyclohexanone and methyl isobutyl ketone to obtain a coating liquid of a composition for forming a low refractive index layer.
[0111] The coating liquid of the composition for forming a low refractive index layer obtained was applied onto the hard coat layer of the PET film-hard coat layer obtained in 1 using a Mayer bar and dried at 90°C for 1 minute. Next, under a nitrogen atmosphere, ultraviolet light was irradiated using an ultraviolet irradiation device (manufactured by Eye Graphics, product name "Eigrantage ECS-401GX type") under the following conditions to form a low refractive index layer with a thickness of 100 nm. [Ultraviolet light irradiation conditions] Light source: high-pressure mercury lamp Lamp power: 2 kW Conveyor speed: 4.23 m / min Illuminance: 300 mW / cm 2 ・Light intensity: 250mJ / cm 2
[0112] 3. Formation of Heat-Ray Shielding Layer 100 parts by mass of a urethane acrylate prepolymer (manufactured by Arakawa Chemical Industries, Ltd., product name "Beamset 575CB") as an active energy ray-curable component, 150 parts by mass of indium tin oxide (ITO) as an infrared-shielding material, and 3 parts by mass of 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one as a photopolymerization initiator were mixed in a 1:1 (mass ratio) mixed solvent of cyclohexanone and methyl isobutyl ketone to obtain a coating liquid of a composition for forming a heat-ray-shielding layer.
[0113] The obtained coating liquid of the composition for forming a heat ray-shielding layer was applied with a Mayer bar onto the PET film opposite the low refractive index layer of the film produced in 1, and dried at 90°C for 1 minute. Next, under a nitrogen atmosphere, the film was irradiated with ultraviolet light using an ultraviolet irradiation device (manufactured by Eye Graphics, product name "Eigrantage ECS-401GX type") under the following conditions to form a heat ray-shielding layer with a thickness of 3.0 µm. [Ultraviolet light irradiation conditions] Light source: high-pressure mercury lamp Lamp power: 2 kW Conveyor speed: 4.23 m / min Illuminance: 300 mW / cm 2 ・Light intensity: 250mJ / cm 2
[0114] 4. Formation of Pressure-Sensitive Adhesive Layer A pressure-sensitive adhesive composition was obtained by adding 1 part by mass (solid content) of an isocyanate crosslinking agent, Coronate (registered trademark) HL (manufactured by Tosoh Corporation), to 100 parts by mass of a toluene solution (solid content: 40% by mass) of an acrylic copolymer (weight average molecular weight: 400,000) having a monomer composition of n-butyl acrylate (n-BA) / 2-hydroxyethyl methacrylate (2-HEMA) / methacrylic acid (MAAc) = 93.76 / 6.2 / 0.04 (mass ratio).
[0115] The pressure-sensitive adhesive composition was applied to a release liner using a knife coater so that the film thickness after drying would be 20 μm, and then dried to form a pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer was then attached to the heat-ray-shielding layer to obtain a window film consisting of the low refractive index layer-hard coat layer-substrate-heat-ray-shielding layer-pressure-sensitive adhesive layer-release liner.
[0116] Example 2 A window film was obtained in the same manner as in Example 1, except that a PET film (thickness: 125 μm, Cosmoshine (registered trademark) A4360 (manufactured by Toyobo Co., Ltd.)) was used as the transparent substrate.
[0117] Comparative Example 1 A window film was obtained in the same manner as in Example 1, except that each layer was formed to have a laminated structure of low refractive index layer-heat ray shielding layer-substrate-adhesive layer-release liner.
[0118] [Evaluation Method 1: Visible Light Transmittance] The window film from which the release liner had been peeled was measured according to the test method described in JIS A5759:2016 (Films for architectural window glass - Visible light transmittance test). The measurement was performed with the glass surface of the test piece facing the light source.
[0119] [Evaluation Method 2: Infrared Reflectance] The release liner was removed from the window film and the infrared reflectance was measured using a spectrophotometer (Shimadzu UV-3600), and the average infrared reflectance in the range of 780 to 2500 nm was taken as the infrared reflectance.
[0120] [Evaluation method 3: Curl] (Evaluation of the effect of suppressing curling of the pressure-sensitive adhesive sheet) The produced window film was cut into a piece of 10 cm x 10 cm, and the release liner surface was placed on a flat table. The warping of the four corners of the window film from the table was observed and evaluated according to the following evaluation criteria.
[0121] ◯: No change Δ: Edge lifting occurs ×: Curl occurs to the extent that it becomes cylindrical The results are shown in Table 1 below.
[0122]
[0123] From the above results, the window films of the examples had high visible light transmittance, excellent infrared reflectance, and excellent curl suppression. The window film of Example 1 had a thinner substrate than the window film of Example 2, and was therefore superior in curved surface conformability. Thinner substrate thickness tends to cause film curl more severely, but the configuration of the present invention, as shown in Example 1 above, can suppress curling of the window film, making it less likely to lift during installation.
[0124] This application is based on Japanese Patent Application No. 2023-54863, filed on March 30, 2023, the disclosure of which is hereby incorporated by reference in its entirety.
[0125] 10 Window film, 11 Low refractive index layer, 12 Hard coat layer, 13 Substrate, 14 Heat ray shielding layer, 15 Pressure sensitive adhesive layer, 16 Release liner
Claims
1. A window film comprising a low refractive index layer, a hard coat layer, a substrate, a heat ray shielding layer, and an adhesive layer laminated in this order, the low refractive index layer being formed from a composition for forming a low refractive index layer, the composition containing hollow silica particles and an active energy ray curable component, and the heat ray shielding layer being formed from a composition for forming a heat ray shielding layer, the composition containing an infrared shielding metal oxide and an active energy ray curable component.
2. The window film according to claim 1, wherein the thickness of the substrate is 100 μm or less.
3. The window film according to claim 1 or 2, wherein the low refractive index layer is the outermost layer.
4. The window film according to claim 1 or 2, wherein the infrared shielding metal oxide is at least one selected from the group consisting of indium-doped tin oxide, antimony-doped tin oxide and cesium-doped tungsten oxide.
5. The window film according to claim 1 or 2, wherein the hard coat layer and the heat ray shielding layer are disposed adjacent to the substrate.
6. The window film according to claim 1 or 2, wherein the low refractive index layer and the hard coat layer are disposed adjacent to each other.
Citation Information
Patent Citations
Heat ray shielding material and window glass
JP2015118281A
Heat blocking film
WO2021045185A1