Galvanized steel sheet for hot stamp and method for producing the same

The galvanized steel sheet with a controlled composition and manufacturing process addresses the challenge of achieving high strength and corrosion resistance while preventing LME cracking, resulting in improved tensile strength and productivity.

WO2024203603A1PCT designated stage expired Publication Date: 2024-10-03KOBE STEEL LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010713
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-02-19
Filing Date
2024-03-19
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional zinc-based galvanized steel sheets for hot stamping face challenges in achieving high strength while maintaining corrosion resistance and preventing Liquid Metal Embrittlement (LME) cracking, which affects joint strength and productivity.

Method used

A galvanized steel sheet with a specific composition and manufacturing process, including a base steel composition of C: 0.15-0.50%, Si: 0.02-2.5%, Mn: 0.5-5%, and controlled carbon concentration at the interface to suppress LME cracking, combined with a hot-dip galvanizing process to ensure high tensile strength and corrosion resistance.

Benefits of technology

The solution provides a galvanized steel sheet with excellent LME resistance and high tensile strength, maintaining corrosion resistance and improving productivity by suppressing carbon concentration at the interface and optimizing the zinc plating layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010713_03102024_PF_FP_ABST
    Figure JP2024010713_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The base steel sheet of this galvanized steel sheet has a component composition that satisfies C: 0.15-0.50 mass%, Si: 0.02-2.5 mass%, Mn: 0.5-5 mass%, P: 0.03 mass% or less (including 0 mass%), S: 0.02 mass% or less (including 0 mass%), Al: 0.010 to 1 mass%, Ti: 0.005-0.080 mass%, and B: 0.0005-0.005 mass%, with the balance being Fe and inevitable impurities. When an element analysis is performed in the thickness direction of the plating layer from the surface of the plating layer by glow discharge optical emission spectrometry (GD-OES), it is found that the carbon concentration [Cf] (mass%) at a position where the concentration of Zn constituting the plating layer is 1.0 mass% and the bulk carbon concentration [Cb] (mass%) satisfy formula (1): [Cf] ≤ 0.65 × [Cb].
Need to check novelty before this filing date? Find Prior Art

Description

Zinc-based coated steel sheet for hot stamping and manufacturing method thereof

[0001] The present disclosure relates to a zinc-based coated steel sheet for hot stamping and a method for producing the same.

[0002] There has been a demand for improved occupant safety in vehicles, and for this purpose, the strength of vehicle body materials has been improved. On the other hand, against the backdrop of worsening issues such as global warming, there has been an accelerating movement to improve automobile fuel efficiency. It is known that reducing the weight of vehicle bodies is an effective way to improve fuel efficiency.

[0003] Steel sheets for hot stamping (hot forming) can easily achieve both high strength and formability (shape fixability, etc.) for the purpose of, for example, realizing vehicle body weight reduction. Hot-dip galvanized steel sheets for hot stamping are used in areas where corrosion resistance is particularly required.

[0004] The following steel sheets have been proposed as the above-mentioned steel sheets for hot stamping (hot forming). For example, Patent Document 1 discloses a steel sheet for hot forming, in which the relationship between Ti and N is specified, which is excellent in the strength of the joint when spot welded and which can achieve good forming without the occurrence of fractures or cracks during hot forming. Furthermore, Patent Document 2 discloses a steel sheet for hot stamping, which is excellent in both the balance of strength and toughness and the hardness stability, in which the proportions of alloy elements are increased to achieve high strength, for example by adjusting the balance of the contents of C, Si, Mn, and Cr.

[0005] However, as the proportion of alloying elements in a zinc-based coated steel sheet increases, cracking due to molten metal embrittlement (LME Liquid Metal Embrittlement or LMC Liquid Metal Cracking) (LME cracking) is likely to occur. In particular, if LME cracking occurs when the zinc-based coated steel sheet is hot stamped and formed into a part, and then spot welded for vehicle body assembly, there is a problem that the joint strength of the welded part is insufficient. In response to this problem, for example, Patent Document 3 discloses that in a formed product obtained by hot stamping a galvannealed steel sheet, the heating time in a furnace (furnace time) needs to be about 4 minutes or more in order to improve weldability and chemical conversion treatability and to suppress LME, and that since hot stamping is inferior in press productivity to cold pressing, there is a demand for a reduction in the furnace time. In light of this, it is proposed to increase the Fe concentration of the galvannealed coating in a galvannealed steel sheet for hot stamping to more than 8.0 mass %, and to reduce the coating weight (Zn content of 15.0 to 40.0 g / m) in order to avoid the time required for forming an Fe-Zn solid solution phase. 2 ) to increase the melting point of the plating.

[0006] JP 2007-169679 A JP 2019-173158 A JP 2022-131411 A

[0007] Kimitaka Hayashi et al., "Behavior of the corrosion tip in under-film corrosion of Zn-Fe alloy plated steel sheets," Iron and Steel, 76th year (1990), No. 9, pp. 1496-1503

[0008] Although the technology of Patent Document 3 can suppress LME, the reduced coating weight of the coating reduces the effective zinc content that contributes to ensuring the corrosion resistance of the coating, making it difficult to achieve the intended role of the coating, which is to improve corrosion resistance. Regarding the corrosion resistance of coatings, as shown in Non-Patent Document 1, it is known that corrosion resistance is significantly deteriorated, particularly when the Fe concentration in the coating exceeds 65 mass%. Therefore, it has been desired to simultaneously achieve high strength, suppression of LME, and ensuring corrosion resistance. The present disclosure has been made in view of the above circumstances, and its purpose is to provide a zinc-based coated steel sheet for hot stamping that exhibits excellent LME resistance while maintaining the inherent corrosion resistance of the coating, and further exhibits high strength (particularly a tensile strength of 1.5G class or more) after hot stamping, and a manufacturing method thereof.

[0009] A first aspect of the present invention is a zinc-based plated steel sheet for hot stamping, wherein the base steel sheet has a chemical composition of C: 0.15 to 0.50 mass%, Si: 0.02 to 2.5 mass%, Mn: 0.5 to 5 mass%, P: 0.03 mass% or less (inclusive of 0 mass%), S: 0.02 mass% or less (inclusive of 0 mass%), Al: 0.010 to 1 mass%, Ti: 0.005 to 0.080 mass%, and B: 0.0005 to 0.005 mass%, with the balance being Fe and inevitable impurities, and wherein, when elemental analysis is performed by glow discharge optical emission spectroscopy (GD-OES) from the surface of the plated layer in the thickness direction of the plated layer, the carbon concentration [Cf] (mass%) at a position where the concentration of Zn constituting the plated layer is 1.0 mass% and the bulk carbon concentration [Cb] (mass%) satisfy the following formula (1): [Cf]≦0.65×[Cb]...(1)

[0010] A second aspect of the present invention is the zinc-based plated steel sheet for hot stamping according to the first aspect, wherein the base steel sheet has a chemical composition that satisfies one or more of the following (a) and (b): (a) further contains one or more elements selected from the group consisting of Cr: more than 0% by mass and not more than 1.2% by mass, Mo: more than 0% by mass and not more than 1% by mass, and Ca: more than 0% by mass and not more than 0.0040% by mass, (b) further contains one or more elements selected from the group consisting of Nb: more than 0% by mass and not more than 0.040% by mass, V: more than 0% by mass and not more than 0.30% by mass, Cu: more than 0% by mass and not more than 0.30% by mass, Ni: more than 0% by mass and not more than 0.30% by mass, Mg: more than 0% by mass and not more than 0.010% by mass, and REM: more than 0% by mass and not more than 0.010% by mass.

[0011] A third aspect of the present invention is a method for producing a zinc-based plated steel sheet for hot stamping, the method comprising: an annealing step in which a hot-rolled steel sheet or a cold-rolled steel sheet satisfying the chemical composition according to the first or second aspect is allowed to remain in a reducing atmosphere having a dew point of −20° C. to +10° C. at 500 to 930° C. for 90 to 1000 seconds; and a subsequent zinc-based plating step.

[0012] A fourth aspect of the present invention is the method for producing a zinc-based plated steel sheet for hot stamping according to the third aspect, wherein the zinc-based plating step is a hot-dip galvanizing step.

[0013] According to the present disclosure, it is possible to provide a high-strength zinc-based plated steel sheet for hot stamping that is excellent in LME resistance and a method for manufacturing the same.

[0014] FIG. 1 is a diagram showing the sampling position of an evaluation steel sheet in an example. FIG. 2 is a diagram showing the carbon profile of a sample before hot stamping in an example, with the left being the carbon profile of a comparative example and the right being the carbon profile of an example of the present invention. FIG. 3 is an SEM photograph showing an example of an EDX analysis area of ​​a sample before hot stamping in an example. FIG. 4 is a diagram showing the EDX analysis results of a sample before hot stamping in an example. FIG. 5 is a diagram showing the heat pattern of hot stamping in an example. FIG. 6 is a diagram showing the carbon profile of a sample after hot stamping in an example, with the left being the carbon profile of a comparative example and the right being the carbon profile of an example of the present invention. FIG. 7 is an SEM photograph showing an example of an EDX analysis area of ​​a sample after hot stamping in an example. FIG. 8 is a diagram showing the EDX analysis results of a sample after hot stamping in an example. FIG. 9 is a diagram showing the conditions of a welding test in an example. FIG. 10 is a diagram explaining the sampling position of a sample for a welding test in an example. FIG. 11 is a diagram explaining the crack observation position of a cross section of a sample after a welding test in an example. FIG. 12 is a diagram explaining internal cracks and voids after a welding test in an example.

[0015] The present inventors conducted extensive research to obtain a zinc-based coated steel sheet for hot stamping that exhibits high strength after hot stamping and also has excellent LME resistance, on the premise that a zinc-coated layer is formed to ensure corrosion resistance. The inventors first conducted research and found that, unlike general cold-rolled steel sheets, a phenomenon occurs in which carbon (C) concentrates at the interface between the coating layer and the steel substrate (hereinafter referred to as the "coated steel substrate interface") when the steel substrate is heated during hot stamping. (As shown in the carbon profile on the left in Figure 6 (described later), the carbon concentration [C] at the coated steel substrate interface after hot stamping, 0.303 mass %, is higher than the carbon concentration of 0.220 mass % in the bulk.) Carbon is known to be an element that deteriorates LME resistance, and the inventors first identified that the main cause of the deterioration of LME resistance in steel sheets for hot stamping is this carbon concentration phenomenon.

[0016] The inventors have also found that, in order to suppress the phenomenon of carbon concentration at the interface between the plated steel and the base steel after hot stamping, it is important to suppress the carbon concentration at the interface between the plated steel and the base steel of the zinc-based plated steel sheet to be subjected to hot stamping, specifically, to satisfy the following formula (1): [Cf]≦0.65×[Cb] (1) In formula (1), [Cf] is the carbon concentration (mass%) at a position where the concentration of Zn constituting the plated layer is 1.0 mass% when elemental analysis is performed from the surface of the plated layer in the thickness direction of the plated layer by glow discharge optical emission spectroscopy (GD-OES), and [Cb] is the bulk carbon concentration (mass%).

[0017] In the above formula (1), "the position where the concentration of Zn constituting the plating layer is 1.0 mass % when elemental analysis is performed from the surface of the plating layer in the thickness direction of the plating layer by glow discharge optical emission spectroscopy (GD-OES)" refers to the interface with the plated steel substrate in this embodiment. In other words, the zinc plating layer refers to the region from the surface of the plating layer where the concentration of zinc (Zn) is 1 mass % or more. The elemental analysis performed from the surface of the plating layer in the thickness direction of the plating layer by glow discharge optical emission spectroscopy (GD-OES) is performed by the method shown in the examples.

[0018] The bulk carbon concentration [Cb] (mass%) refers to the carbon (C) concentration determined by analyzing a steel sheet for hot stamping having a size of total sheet thickness × 50 mm × 50 mm or more using a combustion-infrared absorption method. To determine the bulk carbon concentration, the content of each bulk element may be analyzed using a conventional method, as described below. Since the steel sheets manufactured in the examples described below had an Si content of more than 0.7 mass%, the Si content was determined by the gravimetric method as shown below. However, when the Si content is 0.7 mass% or less, analysis by ICP is recommended. <Analysis methods> Inductively coupled plasma atomic emission spectroscopy (ICP): Si (if 0.7% by mass or less), Mn, P, Cu, sol-Al, Ni, Cr, Mo, V, Nb, Ti, B, Ca Flameless atomic absorption spectroscopy: Sn Gravimetric method: Si (if more than 0.7% by mass) Combustion-infrared absorption method: C, S Inert gas fusion-TCD method [N], inert gas fusion-infrared absorption method [O]: N, O

[0019] The present inventors have discovered that, as shown in the above formula (1), by reducing the carbon concentration at the interface between the galvanized and steel substrates in the surface region of a zinc-based plated steel sheet before hot stamping to [bulk carbon concentration × 0.65] or less, i.e., by providing a surface decarburized layer, the carbon concentration at the interface between the galvanized and steel substrates after hot stamping can be suppressed to approximately the same as the bulk carbon concentration, 0.225 mass%, as shown in the carbon profile on the right side of Figure 6 (described later). As a result, as shown in the examples (described later), LME cracking was suppressed even when welding was performed using the galvanized steel sheet. This suggests that reducing the carbon content in the surface region of the zinc-based plated steel sheet before hot stamping can suppress the carbon enrichment phenomenon after hot stamping, thereby improving LME resistance. In the surface region of the zinc-based plated steel sheet before hot stamping, the carbon concentration at the interface between the galvanized and steel substrates is preferably 0.60 or less of the bulk carbon concentration, more preferably 0.50 or less of the bulk carbon concentration. From the viewpoint of enhancing LME resistance, a smaller ratio to the bulk carbon concentration is preferable. Note that, taking into consideration the manufacturing conditions, the mechanical properties of the steel sheet after hot stamping, etc., the lower limit of the ratio of the carbon concentration at the interface between the plated steel substrate and the bulk carbon concentration can be about 0.01.

[0020] The reduction in the carbon concentration at the interface with the plated base steel in the zinc-based plated steel sheet before hot stamping can be achieved by manufacturing the steel sheet under the conditions described below.

[0021] [Composition] The composition of the base steel sheet (referring to the portion of the plated steel sheet excluding the plating layer) in the zinc-based plated steel sheet for hot stamping according to this embodiment will be described below. In the zinc-based plated steel sheet for hot stamping according to this embodiment, by satisfying the composition below, it is possible to ensure a strength of 1.5 GPa or more after hot stamping, and also to improve part productivity, plating performance, and LME resistance.

[0022] [C: 0.15 to 0.50 mass%] C is an element effective in improving the strength of steel sheets. To achieve a strength of TS: 1470 MPa or more after hot stamping, the C content must be 0.15 mass% or more. The C content is preferably 0.18 mass% or more, more preferably 0.20 mass% or more. On the other hand, if the C content exceeds 0.50 mass%, high strength is easily achieved, but problems such as an excessive increase in the strength of the base sheet such as a hot-rolled steel sheet and deterioration of weldability occur. C is also an element that adversely affects LME resistance. Therefore, the C content is 0.50 mass% or less, preferably 0.40 mass% or less, more preferably 0.38 mass% or less, and even more preferably 0.35 mass% or less.

[0023] [Si: 0.02 to 2.5 mass%] Si has the effect of suppressing the self-tempering of martensite, making it an effective element for improving hardness stability and, therefore, ensuring productivity during component manufacturing. Furthermore, trace amounts of Si suppress the occurrence of unplated areas during steel sheet manufacturing. To achieve these effects, the Si content is set to 0.02 mass% or more. The Si content is preferably 0.1 mass% or more, more preferably 0.5 mass% or more, and even more preferably 0.7 mass% or more. On the other hand, if the Si content exceeds 2.5 mass%, the Ac3 point rises, leading to an increase in the hot stamping heating temperature during component manufacturing. Furthermore, Si is an element that adversely affects LME resistance. While the cause of this is unclear, research results by the present inventors suggest that it is because Si dissolves in the coating, lowering the melting point of the coating. From these perspectives, the Si content is set to 2.5 mass% or less. The Si content is preferably 2.4 mass% or less, and more preferably 2.2 mass% or less.

[0024] [Mn: 0.5 to 5 mass%] Mn is an element necessary for ensuring hardenability and achieving a strength of TS: 1470 MPa or more after hot stamping. Therefore, the Mn content is set to 0.5 mass% or more. The Mn content is preferably 1.0 mass% or more, more preferably 1.5 mass% or more. On the other hand, an excessive Mn content leads to an unnecessarily high strength increase in the base sheet such as a hot-rolled steel sheet. Mn is also an element that deteriorates LME resistance. Therefore, the Mn content is set to 5 mass% or less. The Mn content is preferably 4.5 mass% or less, more preferably 4.0 mass% or less.

[0025] [P: 0.03 mass% or less (including 0 mass%)] P is an element that is inevitably present as an impurity element. P has a negative effect on toughness and delayed fracture resistance. Therefore, the lower the P content, the better, and the P content is 0.03 mass% or less, preferably 0.010 mass% or less. In this specification, "including 0 mass%" means that it includes an embodiment in which it is not intentionally added, that is, a case in which the content is below the level of an unavoidable impurity (it does not exclude the case in which it is intentionally added).

[0026] [S: 0.02 mass% or less (including 0 mass%)] S is an element that is inevitably present as an impurity element. S has a negative effect on toughness and delayed fracture resistance. Therefore, the lower the S content, the better. The S content is 0.02 mass% or less, preferably 0.010 mass% or less, and more preferably 0.005 mass% or less.

[0027] [Al: 0.010 to 1 mass%] Al is an element that acts as a deoxidizer. To achieve this effect, the Al content is set to 0.010 mass% or more. The Al content is preferably 0.015 mass% or more. On the other hand, if the steel sheet contains too much Al, the hardness after die cooling decreases. In addition, Al 2 O 3 The excessive generation of Al deteriorates low-temperature toughness. Therefore, the Al content is set to 1 mass% or less. The Al content is preferably 0.8 mass% or less, and more preferably 0.1 mass% or less. The Al content here refers to the content of Al in a solid solution state (sol. Al).

[0028] [Ti: 0.005 to 0.080 mass%] Ti exerts the effects of B described below. It has the effect of precipitating and neutralizing N, which adversely affects the solid solution of B, with Ti. Furthermore, when Ti is contained together with B, it increases the amount of B in solid solution, thereby improving resistance to LME cracking. To exert these effects, the Ti content is set to 0.005 mass% or more. The Ti content is preferably 0.010 mass% or more, more preferably 0.015 mass% or more, and even more preferably 0.020 mass% or more. On the other hand, excessive Ti content can cause carbide precipitation, grain refinement, and the like, which unnecessarily increase the strength of the base sheet, such as a hot-rolled steel sheet, and can adversely affect economic efficiency due to poor workability. Therefore, the Ti content is set to 0.080 mass% or less. The Ti content is preferably 0.070 mass% or less, and more preferably 0.060 mass% or less.

[0029] [B: 0.0005 to 0.005% by mass] B is an element necessary for ensuring hardenability and achieving a TS strength of 1,470 MPa or more after hot stamping. It also has the effect of improving the resistance to LME cracking of the weld when welded. While the reason for this effect is unknown, research by the present inventors suggests that it is due to the effect of strengthening the prior γ grain boundaries, which are the initiation points of cracks. To achieve these effects, the B content must be 0.0005% by mass or more. The B content is preferably 0.0010% by mass or more, and more preferably 0.0015% by mass or more. On the other hand, an excessive B content increases the strength of the base sheet, such as a hot-rolled steel sheet, more than necessary, resulting in poor workability and adversely affecting economic efficiency. Therefore, the B content is 0.005% by mass or less. The B content is preferably 0.004% by mass or less, and more preferably 0.003% by mass or less.

[0030] The zinc-based plated steel sheet according to an embodiment of the present invention preferably contains the above-described chemical composition, and in one embodiment of the present invention, the balance is preferably iron and inevitable impurities. Elements introduced due to the conditions of raw materials, materials, manufacturing equipment, etc. are permitted as inevitable impurities. N is also an element that is inevitably present as an impurity element and may be contained, for example, in a range of 0.0100 mass% or less (including 0 mass%). Note that, for example, P and S, the lower the content, the better, and therefore they are inevitable impurities, but there are elements whose composition ranges are separately specified as above. For this reason, in this specification, the term "unavoidable impurities" that constitute the balance is a concept that excludes elements whose composition ranges are separately specified.

[0031] The chemical composition of the steel sheet in this embodiment does not necessarily include the elements described below. Any other elements may be further included as long as the desired properties can be maintained. By including the elements described below as necessary, it is possible to improve, for example, delayed fracture resistance and further improve LME resistance.

[0032] [(a) Further, one or more elements selected from the group consisting of: Cr: more than 0% by mass but not more than 1.2% by mass; Mo: more than 0% by mass but not more than 1% by mass; and Ca: more than 0% by mass but not more than 0.0040% by mass] Cr is an element that can further improve resistance to LME cracking while ensuring hardenability. To achieve this effect, the Cr content is preferably more than 0% by mass, more preferably 0.05% by mass or more. On the other hand, an excessive Cr content deteriorates pickling properties required in the manufacturing process. Furthermore, it leads to an excessive increase in the strength of the base sheet, such as a hot-rolled steel sheet. Therefore, the Cr content is preferably 1.2% by mass or less, more preferably 1.0% by mass or less.

[0033] Mo has the effect of promoting the diffusion of B and suppressing susceptibility to LME. From the viewpoint of exerting this effect, the Mo content is preferably more than 0 mass%, more preferably 0.05 mass% or more. On the other hand, an excessive Mo content leads to an unnecessarily high strength increase in the base sheet such as a hot-rolled steel sheet, which deteriorates workability and has a negative impact on economic efficiency. Therefore, the Mo content is preferably 1 mass% or less.

[0034] Ca is an element that improves delayed fracture resistance by suppressing the formation of MnS, which has a negative effect on delayed fracture resistance. From the viewpoint of exerting this effect, the Ca content is preferably more than 0 mass%, more preferably 0.001 mass% or more. On the other hand, if the Ca content is excessive, the effect saturates and adversely affects economic efficiency, such as increasing costs. Therefore, the Ca content is set to 0.0040 mass% or less.

[0035] [(b) further containing one or more elements selected from the group consisting of Nb: more than 0% by mass and 0.040% by mass or less, V: more than 0% by mass and 0.30% by mass or less, Cu: more than 0% by mass and 0.30% by mass or less, Ni: more than 0% by mass and 0.30% by mass or less, Mg: more than 0% by mass and 0.010% by mass or less, and REM: more than 0% by mass and 0.010% by mass or less]

[0036] Nb forms fine carbides and refines the steel structure through its pinning effect, contributing to improved strength and toughness. To achieve this effect, the Nb content is preferably greater than 0 mass%, more preferably 0.0008 mass% or more. On the other hand, if the steel plate contains excessive Nb, coarse carbides are formed, which become the starting point for fracture and lead to a deterioration in toughness. Therefore, the Nb content is preferably 0.040 mass% or less.

[0037] V forms fine carbides, refines the steel structure through a pinning effect, and contributes to improving strength and toughness. It also has a secondary effect by precipitating during tempering. To achieve these effects, the V content is preferably greater than 0% by mass, and more preferably 0.008% by mass or more. On the other hand, excessive V in the steel sheet forms coarse carbides, which act as fracture initiation sites, resulting in a deterioration in toughness. Therefore, the V content is preferably 0.30% by mass or less.

[0038] Cu and Ni are elements effective in improving the delayed fracture resistance of a component, and may be contained in amounts exceeding 0% by mass as necessary. On the other hand, excessive Cu and Ni in a steel sheet can cause defects on the surface of the steel sheet and ultimately on the surface of the component. For this reason, the individual contents of Cu and Ni are preferably 0.30% by mass or less, and the total content is more preferably 0.50% by mass or less.

[0039] Mg and REM may be added as needed because they have the function of refining inclusions in the steel sheet and preventing cracks caused by the inclusions during hot forming. When added, the content of each element is preferably more than 0 mass%, more preferably 0.0008 mass% or more. On the other hand, even if these elements are contained in excess, the effect saturates and costs increase. Therefore, the content of each element is preferably 0.010 mass% or less, more preferably 0.008 mass% or less. Note that the REM mentioned above includes lanthanoid elements (15 elements from La to Lu), Sc (scandium), and Y (yttrium).

[0040] The type of zinc-based coating in the zinc-based coated steel sheet for hot stamping according to this embodiment is not limited. Examples include Fe-Zn coating and Al-Zn coating. The Fe concentration in the coating layer of the zinc-based coated steel sheet for hot stamping according to this embodiment is preferably 40 mass% or less, and more preferably 30 mass% or less. Specific examples of the zinc-based coated steel sheet include hot-dip galvanized steel sheet (GI), galvannealed steel sheet (GA), and electrogalvanized steel sheet (EG).

[0041] The coating weight of the zinc-based coating (particularly hot-dip galvanizing and galvannealed hot-dip galvanizing) of the zinc-based coated steel sheet for hot stamping according to this embodiment is 45 g / m from the viewpoint of ensuring corrosion resistance. 2 It is preferable that the content is 60 g / m or more, and more preferably 60 g / m 2 More preferably, it is 65 g / m 2 On the other hand, from the viewpoint of easily achieving the recommended Fe concentration in the plating layer, it is preferable that the coating weight of the zinc-based plating is small. Therefore, the coating weight of the zinc-based plating is 190 g / m 2 It is preferable that the density is 180 g / m or less, and more preferably 180 g / m 2 The following is the result.

[0042] The zinc-based plated steel sheet for hot stamping according to this embodiment is subjected to hot stamping by the method described in the Examples below, and the resulting zinc-based plated steel sheet has an Fe concentration of preferably 65% ​​by mass or less, and more preferably 60% by mass or less. Note that, from the viewpoint that the Fe concentration in the plated steel increases by hot stamping, the Fe concentration can be 20% by mass or more.

[0043] According to this embodiment, as described above, the predetermined component composition is satisfied and a predetermined surface decarburization layer is provided, thereby improving LME resistance without reducing the coating weight of the coating or increasing the Fe concentration in the hot-dip galvanized layer.

[0044] [Method for manufacturing zinc-based plated steel sheet for hot stamping] Next, a method for manufacturing a zinc-based plated steel sheet for hot stamping according to this embodiment will be described.

[0045] The method for producing a zinc-based plated steel sheet for hot stamping according to this embodiment includes an annealing step in which a hot-rolled steel sheet or a cold-rolled steel sheet satisfying the above-described chemical composition is allowed to remain in a reducing atmosphere having a dew point of −20° C. to +10° C. at 500 to 930° C. for 90 to 1000 seconds, and a subsequent zinc-based plating step.

[0046] The annealing step and the subsequent zinc-based plating step, which are features of the manufacturing method according to this embodiment, will be described first. Hereinafter, an embodiment in which the annealing step and the subsequent zinc-based plating step (particularly the hot-dip galvanizing step) according to this embodiment are performed in a hot-dip galvanizing line of a reducing furnace type will be described as an example, but the present invention is not limited to this. The method according to this embodiment is not limited to this embodiment, and for example, the hot-dip galvanizing line can also be performed in a continuous annealing line of a non-oxidizing furnace type.

[0047] (Annealing Process) The annealing process of a hot-dip galvanizing line is usually composed of a reducing furnace and a cooling zone. This embodiment is characterized in that the annealing conditions in the reducing furnace, particularly the dew point of the reducing atmosphere, are appropriately controlled. A raw sheet is charged into the reducing furnace. The raw sheet charged into the reducing furnace may be subjected to a pretreatment process, such as degreasing, as described below, as necessary. Furthermore, the raw sheet charged into the reducing furnace may be subjected to an oxidation treatment in an oxidation furnace after the pretreatment process, as necessary.

[0048] In the reduction furnace, the base sheet is subjected to heat treatment in a reducing atmosphere. The dew point of the reducing atmosphere is set to -20°C to +10°C. By setting the dew point within this range, decarburization of the surface layer of the steel sheet occurs, and the desired surface layer region can be obtained. The dew point of the reducing atmosphere is preferably -15°C or higher, more preferably -10°C or higher. The dew point of the reducing atmosphere is also preferably +5°C or lower, more preferably 0°C or lower.

[0049] The dew point can be controlled by, for example, introducing water vapor gas and mixing it with the atmospheric gas in the furnace, or bubbling the atmospheric gas to mix water vapor into it. The reducing atmosphere is not particularly limited as long as it satisfies the dew point and is reducing. The reducing atmosphere is not particularly limited as long as it satisfies the dew point and is reducing, for example, H 2 -N 2 H in the mixed gas 2 The concentration is preferably 1 to 30% by volume.

[0050] The annealing temperature is set to 500 to 930°C, and the residence time at the annealing temperature, i.e., the annealing time, is set to 90 to 1000 seconds. Annealing within the above temperature range is also called soaking treatment, and in this case, the annealing temperature is called the soaking temperature, and the annealing time is called the soaking time.

[0051] The annealing temperature is preferably 530°C or higher, more preferably 560°C or higher, and even more preferably 600°C or higher. The annealing temperature is preferably 900°C or lower, more preferably 870°C or lower. The annealing time is preferably 100 seconds or higher, more preferably 120 seconds or higher. The annealing time is preferably 900 seconds or lower, more preferably 700 seconds or lower, even more preferably 500 seconds or lower, even more preferably 400 seconds or lower, and even more preferably 350 seconds or lower. The annealing time can be controlled by the speed at which the raw sheet passes through the reducing furnace (hereinafter also referred to as "line speed" or abbreviated as "LS"). "Residing at 500 to 930°C for 90 to 1000 seconds" means that the sheet is allowed to stay within the annealing temperature range of 500 to 930°C for 90 to 1000 seconds, and the temperature may be constant or may vary within the above annealing temperature range.

[0052] According to the manufacturing method of this embodiment, a predetermined surface decarburized layer can be provided by particularly performing the above-mentioned annealing on a hot-rolled steel sheet or a cold-rolled steel sheet, which is a base sheet having the above-mentioned component composition.

[0053] A pretreatment process of the base sheet that can be performed before the annealing process will be described. Pretreatment is typically performed to remove oil (grease) and dirt adhering to the surface of the base sheet, typically alkaline degreasing. The alkali contained in the degreasing solution used in alkaline degreasing is preferably, for example, caustic soda, silicate, or a mixture thereof, and is not particularly limited as long as it can remove oil and fat as water-soluble soap. Furthermore, to improve degreasing properties, electrolytic cleaning, scrubber treatment, and addition of a surfactant or chelating agent to the degreasing solution can also be performed. In this embodiment, the pretreatment method is not limited as long as the surface of the base sheet is appropriately degreased, and the above-mentioned treatments may be performed alone or in any combination.

[0054] The raw sheet that leaves the reduction furnace can be cooled in a cooling zone. The cooling zone can be composed of a slow cooling zone, a quenching zone, and an adjustment zone. The adjustment zone is also called a holding zone. Cooling can be carried out under commonly used conditions so as to prevent the occurrence of bare spots, and examples of such methods include cooling the steel sheet by blowing a gas in a reducing atmosphere onto it.

[0055] A hot-dip galvanizing line using a reduction furnace is generally divided into a pretreatment process, an annealing process, and a plating process, in which an alloying process is also carried out as necessary.

[0056] From the viewpoint of energy saving, the pretreated raw sheet may be preheated in a preheating furnace having a reducing or oxidizing atmosphere using exhaust gas after the pretreatment step and before entering the reduction furnace.

[0057] (Zinc-based plating process) After the annealing process (continuous annealing process), a zinc-based plating process is included. Hereinafter, a hot-dip galvanizing process will be described as an example of the zinc-based plating process. A hot-dip galvanized steel sheet (GI) is produced by the hot-dip galvanizing process. Alternatively, the GI may be alloyed to produce a galvannealed steel sheet (GA).

[0058] The hot-dip galvanizing step is not particularly limited, and a commonly used method can be adopted. For example, the temperature of the hot-dip galvanizing bath may be controlled to about 430 to 500°C. The coating weight of the hot-dip galvanized layer (the same as the coating weight of the alloyed hot-dip galvanized layer described below) is set to 45 g / m from the viewpoint of ensuring corrosion resistance. 2 It is preferable that the density is 60 g / m or more, and more preferably 60 g / m 2 More preferably, it is 65 g / m 2 On the other hand, from the viewpoint of easily achieving the recommended Fe concentration in the coating layer, it is preferable that the coating weight of the hot-dip galvanized layer (particularly the alloyed hot-dip galvanized layer) is small. Therefore, the coating weight of the hot-dip galvanized layer is 190 g / m or more. 2 It is preferable that the density is 180 g / m or less, and more preferably 180 g / m 2 The following is the result.

[0059] The alloying treatment is not particularly limited, and a commonly used method can be employed. In the alloying treatment, when the Fe concentration in the plating layer is increased, the alloying temperature can be controlled to, for example, about 400 to 700°C. The alloying temperature is furthermore 430°C or higher, furthermore 440°C or higher, and even furthermore 450°C or higher. On the other hand, if the alloying temperature is too high, the Fe concentration in the plating layer becomes too high, so the alloying temperature is preferably 680°C or lower, more preferably 650°C or lower.

[0060] The steps after the plating step are not particularly limited, and commonly used methods can be adopted. Usually, skin-pass treatment, tension leveling, oiling, etc. are performed, but these may be performed under commonly used conditions as needed, or may not be performed if unnecessary. The galvanized steel sheet (GI or GA) obtained in this manner is suitable for use as a steel sheet for hot stamping.

[0061] Instead of the hot-dip galvanizing, electroplating may be performed. For example, the base sheet may be subjected to the above-described annealing and then electroplated to obtain an electrogalvanized steel sheet having the galvanized base steel interface specified in this embodiment.

[0062] (Other Steps) The manufacturing method according to this embodiment may include the specified annealing step and the subsequent zinc-based plating step. The other steps are not limited and may include commonly performed steps. Therefore, the manufacturing method of the hot-rolled or cold-rolled steel sheet subjected to the annealing step is not limited. For example, the hot-rolled or cold-rolled steel sheet can be manufactured as follows. First, a slab is manufactured. In the slab manufacturing step, steel is melted according to a conventional method, and the molten steel is poured into a mold for continuous casting to obtain a slab. In this step, the composition of the steel is adjusted during melting so as to satisfy the above-mentioned composition ranges. After casting and before hot rolling, a heating step may be performed to prevent cracks from occurring during hot rolling (this step is different from the slab heating step in the hot rolling step described below). The heating conditions are not particularly limited, and commonly used conditions can be appropriately adopted. However, it is preferable to perform the heating at a temperature of approximately 1100°C to 1300°C.

[0063] In the hot rolling process, the slab is first placed in a heating furnace and heated to a predetermined temperature (generally 1100°C to 1300°C, for example, 1200°C), and then held at that temperature for a predetermined time (for example, 30 minutes).

[0064] The heated slab is then placed upstream of the hot rolling line and rolled into a steel plate having a predetermined thickness by passing the slab between the rolls of the rolling stands of the roughing mill and the finishing mill in succession. After hot rolling, the steel plate is cooled to a predetermined temperature in a cooling device and then wound up by a coiler.

[0065] The hot-rolled steel sheet may be a hot-rolled pickled steel sheet that has been subsequently pickled in a pickling process. The pickling process is sufficient as long as at least the hot-rolling scale is removed by pickling. The hot-rolled pickled steel sheet may be cold-rolled as needed. In the cold-rolling process, the hot-rolled steel sheet is further rolled to reduce its thickness. Specifically, the hot-rolled steel sheet after pickling is passed between rolls in a rolling stand to further reduce its thickness. Cold-rolled steel sheets are particularly suitable for use in automotive parts aimed at reducing the weight of automobiles. From the viewpoints of dimensional accuracy and flatness, it is desirable that the base steel sheet constituting the zinc-based plated steel sheet be a cold-rolled steel sheet. The hot-rolled steel sheet (including the hot-rolled pickled steel sheet) or cold-rolled steel sheet (hereinafter collectively referred to as "base sheet") may be subjected to the annealing process and a zinc-based plating process, for example, a continuous plating process using a reduction furnace.

[0066] The present disclosure will be described in more detail below with reference to examples. The present disclosure is not limited to the following examples, and can be implemented by making appropriate modifications within the scope of the above-mentioned and below-mentioned aims, and all such modifications are included in the technical scope of the present disclosure.

[0067] Steel materials having the chemical compositions shown in Table 1 were melted in a converter and then continuously cast into slabs. The resulting slabs were heated to temperatures of 1100°C to 1300°C and then hot-rolled under conditions of an FDT of 890°C to 950°C and a coiling temperature of 500°C to 700°C. The slabs were then descaled in a pickling process and cold-rolled to obtain cold-rolled steel sheets. The cold-rolling reduction ratio was 20% or more. The resulting cold-rolled steel sheets had a thickness of 1.2 mm. In this example, plated steel sheets were produced using the cold-rolled steel sheets as base sheets. Note that underlined values ​​in Table 1 indicate values ​​outside the range specified in this embodiment. The same applies to the following tables. Steel type 2 in Table 1 is a comparative steel type due to its low carbon (C) content.

[0068]

[0069] The obtained cold-rolled steel sheets were subjected to reduction annealing in a hot-dip galvanizing annealing line under the conditions (soaking temperature (annealing temperature), soaking time (annealing time), dew point) shown in Table 2. In Experiments 1 to 7, after immersion in the galvanizing bath, alloying was performed under the conditions (alloying temperature, alloying time) shown in Table 2 to obtain galvannealed steel sheets (GA steel sheets) with a width of approximately 1000 mm and coated on both sides with galvannealed hot-dip galvanizing. The GA steel sheets are also steel sheets for hot stamping. These GA steel sheets are sometimes referred to as "steel sheets before hot stamping." In Experiments 8 to 10, small samples of 150 mm x 80 mm were used to perform galvanizing (decarburization) annealing. It was separately confirmed that these small samples had the same decarburization state and strength as the above-mentioned steel sheets. In Experiments 8 to 10, the coating weight was not measured. A separate evaluation of materials annealed under the same conditions yielded a coating weight of 180 g / m 2 Therefore, it is assumed that the same plating coating weight (weight per unit area) is also attached in Experiments No. 8 to 10, and in Table 2, 2 It shows:

[0070]

[0071] In Experiments No. 1 to 7, evaluation steel sheets measuring 150 mmW x 70 mmL or 220 mmW x 150 mmL were sampled from the GA steel sheet at positions a in the center (within the width direction W / 4 to 3W / 4) and b in the edge (the region furthest from the edge) in Figure 1. The sampled positions for the evaluation steel sheets in each example are shown in Table 5. In Experiments No. 8 to 10, the small samples (size: 150 mmW x 80 mmL) obtained above were used without cutting.

[0072] Using each evaluation steel sheet, the decarburization state of the surface layer of the steel sheet and the Fe concentration in the plating layer before hot stamping were measured as follows.

[0073] [Measurement of Decarburization State of Surface Layer (Before Hot Stamping) (Carbon Profile Measurement by GD-OES)] Carbon profile measurement was carried out by GD-OES (Glow Discharge Optical Emission Spectrometry) as described below to investigate the decarburization behavior.

[0074] (Sample Preparation) Materials measuring 50 mm x 40 mm x 1.2 mm (total thickness), 30 mm x 30 mm x 1.2 mm (total thickness), or 30 mm x 40 mm x 1.2 mm (total thickness) were collected. Then, degreasing was performed as usual to prepare samples. Using these samples, the mass % concentration of each element was measured using GD-OES under the following conditions.

[0075] (Measurement conditions) Equipment used: Marcus-type radio frequency glow discharge optical emission surface analyzer (rf-GD-OES) GD-Profiler 2 manufactured by HORIBA, Ltd. Sputtering method: normal sputtering Measurement range: φ4 mm Type of gas: Ar Elements to be analyzed: B, C, O, Al, Si, Ti, Cr, Mn, Fe, Zn, P, S, N (In this example, the evaluation was performed on these elements, but if elements other than those listed above are contained in, for example, the plating layer or steel sheet, the elements other than those listed above will also be analyzed.)

[0076] (Measurement Method) GD-OES measurements were carried out on the plated surface of the sample up to a depth of 150 μm in the thickness direction.

[0077] (Analysis Method) Since the sputtering rate of this device is almost constant, the sputtering crater depth of the sample was measured after the analysis was completed, and the horizontal axis was set to this value (sputtering depth).

[0078] The details of the calibration curve method for converting the measured emission intensity of each element into a concentration are shown below. i (g / sec) and luminescence intensity I i The relationship between W and W is expressed by the following formula (I) using the slope a and intercept b of the calibration curve. i = aI i + b Formula (I) Sputter weight W of the element i per unit time i is the concentration C i (wt.%), density ρ (g / cm 3 ), and for a reference sample with a known sputtering rate Δd (cm / sec), the sputtering area S (cm 2 ) and is calculated by the following formula (II): i =C i ×ρ×Δd×S...Formula (II)

[0079] W i Using two or more reference samples with known emission intensities I i The slope a and intercept b of the above formula (I) were determined, and a calibration curve was prepared in which the horizontal axis represents the emission intensity and the vertical axis represents the sputter weight. The reference samples used are shown in Table 3 below. Using the prepared calibration curve, the sputter weight was calculated from the emission intensity of each target element, and the weight ratio was used to convert it into a concentration. The calibration curve used to convert the O concentration was 2 Correction was performed using the formula so that the concentration ratio of Si to O became 1:2.

[0080]

[0081] From the above analysis results, a zinc and carbon profile was obtained, which was the result of analyzing zinc and carbon. From the zinc and carbon profile, the carbon concentration [Cf] at the position where the Zn concentration constituting the plating layer was 1.0 mass% was determined. The bulk carbon concentration [Cb] was determined by the analysis described above. The value of [Cf] / [Cb] was then calculated. The results are shown in Table 5.

[0082] As examples of the carbon profile, the carbon profile of Experiment No. 4, which is a conventional steel as a comparative example, is shown on the left side of Figure 2, and the carbon profile of Experiment No. 1, which is an example of the present invention, is shown on the right side of Figure 2. Comparing these carbon profiles, it can be seen that the carbon concentration at the interface between the coating layer and the base steel sheet is sufficiently suppressed in the example of the present invention.

[0083] Note that the carbon concentration at the steel substrate-coating interface was not evaluated in Experiment No. 6. However, because the chemical composition was the same as in Experiment No. 7 and the reduction annealing conditions were similar, the carbon concentration at the steel substrate-coating interface is thought to be similar to that of Experiment No. 7. Therefore, the carbon concentration at the steel substrate-coating interface in Experiment No. 6 is estimated to be approximately 0.070, the same as in Experiment No. 7, and this value is entered in Table 5.

[0084] [Measurement of Fe concentration in coating layer (before hot stamping)] A sample measuring 20 mm W x 10 mm L x thickness was cut and collected from the above GA steel sheet (steel sheet before hot stamping). Degreasing was performed as necessary.

[0085] <Preparation of Observation Sample> The specimen was embedded in resin so that the L-direction cross section, that is, the surface defined by the plate thickness and 10 mm L, served as the observation surface, and after polishing, gold vapor deposition was performed.

[0086] <SEM Observation> SEM observation and EDX analysis were carried out under the following conditions. In this example, the observation magnification was set to 1500x, but since the observation magnification depends on the amount of plating applied, it is advisable to select an appropriate magnification for measuring the Fe concentration, for example, by lowering the measurement magnification as the plating thickness increases. (SEM Observation Conditions) - Apparatus: Carl Zeiss Field Emission Scanning Electron Microscope (FE-SEM) Supra-35 - Observation image: Backscattered electron image - Observation location: Near the surface including the plating layer - Observation magnification: 1500x - Number of observation fields: 1 field representing the sample / 1 sample

[0087] <EDX Analysis> - Apparatus: Oxford Energy Dispersive X-ray (EDX) Detector X-max80 - Analysis Method: Area Analysis (Qualitative / Semi-Quantitative Analysis) - Analysis Location: Entire plating layer; an example of the analysis area is shown in Figure 3. - Number of Analyzed Fields: One field representing the sample / one sample - Analyzed Elements: The Fe concentration (%) was calculated as the mass % of Fe evaluated when all elements detected by EDX, excluding C, were used as the population. As an example, the analysis results for Experiment No. 4 are shown in Figure 4. Also, as an example, the calculation results for the Fe concentration (12.0 mass %) for Experiment No. 4 are shown in Table 4. The Fe concentration in the plating layer for each example, calculated in the same manner as in Table 4 below, is shown in Table 5.

[0088]

[0089]

[0090] [Evaluation of Steel Sheets After Hot Stamping] To evaluate the steel sheets after hot stamping, the above-mentioned steel sheets for evaluation were subjected to hot stamping as follows. First, to prevent carburization during hot stamping, the steel sheets were degreased in a conventional manner. Next, hot stamping was performed under the following conditions and according to the heat pattern shown in Figure 5 to obtain hot stamped samples.

[0091] (Hot stamping conditions) Sample size: 150mmW x 70mmL, 150mmW x 220mmL, or 150mmW x 80mmL (small sample) Mold used: Flat plate mold <Heating conditions> Air atmosphere electric furnace set temperature: 910°C Heating time: After the plate temperature reached 870°C, it was held for 45 seconds (during which the plate temperature was controlled to be between 870°C and 900°C). <Cooling conditions> After that, it was allowed to cool naturally, and when the plate temperature reached 550°C or 700°C, both flat surfaces were pressed with a flat plate mold to cool. Press load: 0.5MPa Press speed: 20spm Push-in depth: 5mm Bottom dead center holding time: The bottom dead center was held until the temperature dropped below 50°C (10 seconds in this case).

[0092] The hot stamped samples were used to evaluate the tensile strength TS, LME resistance, etc., as described in detail below.

[0093] [Shot Blasting] The surface resistance of the hot stamped samples was measured in accordance with the method described in ISO-18594:2007(E). Shot blasting was performed under the following resistance measurement conditions so that the surface resistance would be 2.0 mΩ or less. The respective shot blasting conditions are shown in Table 6. Note that in Experiments 8 to 10, the resistance after shot blasting was not measured. However, since the average resistance of materials prepared under approximately the same conditions (Experiments 1 to 5) was 0.9 mΩ, it is assumed to be approximately the same, and is shown as 0.9 (mΩ) in Table 6 below.

[0094] (Shot blasting conditions) Shot material: GH-3 (grid 0.3 mm) Shot pressure: approximately 0.4 MPa Shot time per 150 mm x 120 mm area was controlled (details of shot blasting time are given in Table 6) Shot blasting was performed on both sides Shot blasting was performed until the resistance value of the steel plate reached 2.0 mΩ or less.

[0095] (Resistance measurement conditions) - Three pieces of material measuring 30 mm x 30 mm x thickness were cut and collected. - Electrode material: Cu-Cr - Electrode diameter: Φ8 mm - Tip R: 40 mm - DC current value: 2 A - Pressure: 350 ± 17.5 x 10 N - However, measurements were limited to one per sample, with a total of three measurements taken for each experimental sample. - The average value of N3 was used as the value. - The plated side of one steel sheet was clamped between the electrodes and measured. - The resistance value was calculated by subtracting the setup resistance from the total (total) resistance.

[0096]

[0097] [Measurement of Decarburization State of Surface Layer After Hot Stamping (Carbon Profile Measurement by GD-OES)] Carbon profiles were measured by GD-OES (Glow Discharge Optical Emission Spectrometry) as described below to investigate the decarburization behavior after hot stamping.

[0098] (Sample Preparation) Materials measuring 30 mm x 90 mm x thickness or 30 mm x 70 mm x thickness were collected. They were then degreased as per usual methods to prepare samples. Using these samples, the mass % concentration of each element was measured using GD-OES under the following conditions.

[0099] (Measurement conditions) Equipment used: Marcus-type radio frequency glow discharge optical emission surface analyzer (rf-GD-OES) GD-Profiler 2 manufactured by HORIBA, Ltd. Sputtering method: normal sputtering Measurement range: φ4 mm Type of gas: Ar Elements to be analyzed: B, C, O, Al, Si, Ti, Cr, Mn, Fe, Zn (In this example, the evaluation was performed on these elements, but if elements other than those listed above are contained in, for example, the plating layer or steel sheet, the elements other than those listed above will also be analyzed.)

[0100] (Measurement Method) GD-OES measurements were carried out on the plated surface of the sample up to a depth of 100 μm in the thickness direction.

[0101] (Analysis Method) Analysis was carried out using the same method as in the measurement of the decarburization state of the surface layer (before hot stamping) (measurement of the carbon profile by GD-OES) described above.

[0102] Using hot-stamped samples, carbon profiles were measured by GD-OES under the conditions described above to investigate decarburization behavior. As an example, the carbon profile of Experiment No. 4, a conventional steel used as a comparative example, is shown on the left in Figure 6, while the carbon profile of Experiment No. 1, an example of the present invention, is shown on the right in Figure 6. Comparing these carbon profiles, as shown in Figure 6 by the vertical double-headed arrows indicating the difference in carbon concentration at the interface between the coating layer and the base steel sheet, reveals that in the example of the present invention, the carbon concentration at the interface between the coating layer and the base steel sheet is sufficiently suppressed even after hot stamping. In Table 8, a "-" next to the C concentration at the base steel-coating interface indicates that it was not measured.

[0103] [Measurement of Fe Concentration in Coating Layer After Hot Stamping] The Fe concentration in the coating layer after hot stamping was measured in the same manner as the measurement of the Fe concentration in the coating layer before hot stamping. An example of an analysis area for EDX analysis in measuring the Fe concentration in the coating layer after hot stamping is shown in FIG. 7 . As an example of EDX analysis, the analysis results of Experiment No. 4 are shown in FIG. 8 . Furthermore, as an example, the calculation results of the Fe concentration (53.4 mass%) in Experiment No. 4 are shown in Table 7. The Fe concentration in the coating layer of each example, calculated in the same manner as in Table 7 below, is shown in Table 8.

[0104]

[0105] [Tensile Test] Using the hot stamped sample, a tensile test was performed under the following conditions to measure the tensile strength (TS, unit: MPa). (Test Specimen Preparation) For a material measuring 150 mmW x 70 mmL x plate thickness, 150 mmW x 220 mmL x plate thickness, or 150 mmW x 80 mmL (small sample), a 150 mmW x 30 mmL sample for specimen collection was taken from the center of the plate. JIS No. 5 test specimens were then prepared from the 150 mmW x 30 mmL test specimen samples. (Tensile Test Method) Using the above JIS No. 5 test specimens, the tensile strength (TS, unit: MPa) was measured at a strain rate of 10 mm / min using a Shimadzu AG-IS 250kN autograph tensile tester in accordance with the method specified in JIS Z 2241.

[0106] [Welding Test] The hot stamped sample was cut to prepare a plurality of welding test samples measuring 30 mm × 30 mm × plate thickness, and a welding test was performed under the following conditions and as shown in Fig. 9. In Fig. 9, X in "XkA" in the 2nd pulse (second current) represents 15 current conditions changed in 0.5 kA increments between 5.0 kA and 12.0 kA as shown below.

[0107] <Welding conditions> - Pre-weld: To allow the tip to settle in well before the actual welding, 20 welds were made at 6.5 kA on a pair of mild steel sheets. Other conditions for the pre-weld and the actual welding were as follows: Welding time: 10 cycles Pressure: 1.7 kN Hold time: 1 cycle - Actual welding: Name of equipment: Servo pressure spot welding equipment Manufacturer: Nastoa Welding Technology Co., Ltd. Electrode: Upper and lower dome radius type Cu-Cr Electrode diameter: Outer diameter Φ16 mm, tip diameter: Φ6 mm Welding angle: 0° Cooling water flow rate: Approximately 2 liters / min. up and down Pressure: 500 kgf Initial weld time: 60 cycles / 60 Hz Upslope: 1 cycle / 60 Hz First weld: Welding time: 36 cycles / 60 Hz Current value: 4.5 kA Second weld: 18 cycles / 60 Hz Current values: 5.0 kA, 5.5 kA, 6.0 kA, 6.5 kA, 7.0 kA, 7.5 kA, 8.0 kA, 8.5 kA, 9.0 kA, 9.5 kA, 10.0 kA, 10.5 kA, 11.0 kA, 11.5 kA, 12.0 kA Hold time: 10 cycles / 60 Hz <Sheet combination> - Two-sheet combination The upper and lower sheets were the same type of steel sheets - Test specimens were prepared to perform the second current flow n1 for a total of 15 current conditions.

[0108] [Evaluation of LME Cracking] A test piece for evaluating LME cracking was prepared from the sample (welded test piece) after the above-mentioned welding test as follows. Fig. 10 is a schematic top view of Sample 1 after the welding test, in which the upper and lower plates were welded. The shaded area in Fig. 10 (including part of nugget 3) was taken from Sample 1 after the welding test as Test Piece 2 for evaluating LME cracking. When taking the test piece, first, taking into account the polishing allowance, the specimen was cut at cutting surface 4 so that the center of nugget 3 (diameter surface of the nugget) could be photographed, and then polished so that the center of the nugget (diameter surface of the nugget) became the observation surface 5.

[0109] Next, the observation surface 5 was subjected to a conventional corrosion treatment so that the HAZ and nugget diameter could be identified. Then, for all samples, cross-sections were photographed at a magnification that covered the HAZ (photographs were taken in the direction of the white arrow in Figure 10). An example of a photograph is shown in Figure 11. This photograph was taken at a magnification of 25x. Since there were 15 current conditions for one experiment, 15 LME crack evaluation samples were photographed for one experiment.

[0110] For each current condition, cracks were observed at eight locations (1) to (8) shown in Figure 11. In other words, a total of 120 cracks were confirmed at 15 current conditions x 8 locations. The total number of locations where cracks with lengths of 300 μm or more were confirmed was calculated. Note that (1) to (6) in Figure 11 were likely to be cracks extending from the surface generally in the thickness direction (surface cracks), while (7) and (8) in Figure 11 were likely to be cracks extending generally toward the center of the nugget (internal cracks). Note that void Q shown in Figure 12 is not a crack. Internal cracks R extending from void Q shown in Figure 12 were counted.

[0111] These results are shown in Table 8. In the properties shown in Table 8, when the tensile strength TS after hot stamping was 1470 MPa or more and the cracking evaluation result after the welding test (the total number of locations where LME cracks were confirmed) was 3 or less, the specimen was deemed to be an inventive example having high strength and excellent LME resistance. The tensile strength TS may further be 1500 MPa or more, even more preferably 1550 MPa or more, or even more preferably 1600 MPa or more. On the other hand, specimens in which at least one of the strength and the cracking evaluation result after the welding test did not satisfy the above evaluation criteria were deemed to be comparative examples. In this embodiment, specimens in which the Fe concentration in the coating layer was 65% by mass or less were deemed to have excellent corrosion resistance. The measurement results of the Fe concentration in the coating layer are also shown in Table 8.

[0112]

[0113] The above results reveal the following. Experiments Nos. 1 to 3, 8, and 9 satisfied the chemical composition and manufacturing conditions (reduction annealing conditions) specified in this embodiment, and as a result, the tensile strength (TS) after hot stamping was 1,470 MPa or more. Furthermore, the carbon concentration in the surface layer of the steel sheet before hot stamping satisfied formula (1), and excellent LME resistance was demonstrated, with three or fewer LME cracks confirmed after welding. Note that in this example, LME resistance was evaluated by a welding test after hot stamping, but LME resistance is also a property required during hot stamping, which involves high temperatures. In other words, LME resistance is also required for hot-dip galvanized steel sheets before hot stamping. Since good hot-stamping was achieved in Experiments Nos. 1 to 3, 8, and 9, the hot-dip galvanized steel sheets for hot stamping in these examples can be said to have excellent LME resistance.

[0114] On the other hand, Experiments Nos. 4 to 7 and 10 did not satisfy at least one of the component composition and manufacturing conditions (reduction annealing conditions) specified in this embodiment, and the desired properties were not obtained.

[0115] Experiments Nos. 4 and 5 satisfied the component composition specified in this embodiment, and the tensile strength after hot stamping was 1,470 MPa or more. However, in these examples, the manufacturing conditions (reduction annealing conditions) were not satisfied, and the dew point during reduction annealing was −20° C. or lower. As a result, the carbon concentration in the surface layer of the steel sheet before hot stamping did not satisfy formula (1). Therefore, the total number of cracks confirmed in the LME resistance evaluation was four or more, resulting in poor LME resistance.

[0116] In Experiments No. 6 and 7, the carbon content in the composition was below the range specified in this embodiment, and therefore the tensile strength (TS) after hot stamping was below 1470 MPa. Note that Experiments No. 6 and 7 did not satisfy the manufacturing conditions (reduction annealing conditions), and the carbon concentration in the surface layer of the steel sheet before hot stamping did not satisfy formula (1). However, in the LME resistance evaluation, the total number of locations where LME cracking was confirmed was three or less. The reason for this is that the bulk components, particularly the carbon content, were quite low.

[0117] Experiment No. 10 satisfied the component composition specified in this embodiment, and the tensile strength after hot stamping was 1,470 MPa or more. However, the manufacturing conditions (reduction annealing conditions) were not satisfied, and the dew point during reduction annealing was −20° C. or less. As a result, the carbon concentration in the surface layer of the steel sheet before hot stamping did not satisfy formula (1). Therefore, the total number of cracks confirmed in the LME resistance evaluation was four or more, resulting in poor LME resistance.

[0118] Table 8 includes some estimated values ​​for Experiments 6 to 10, which will be explained below. First, the carbon concentration at the steel substrate-coating interface after hot stamping in Experiment 6 was not measured. However, Experiment 6 had the same chemical composition as Experiment 7 and similar reduction annealing conditions. Furthermore, the hot stamping heating conditions were also nearly the same, so it is assumed that the carbon concentration at the steel substrate-coating interface would be equivalent to that in Experiment 7. Therefore, the carbon concentration at the steel substrate-coating interface after hot stamping in Experiment 6 is listed assuming that it will be nearly the same as that in Experiment 7.

[0119] Furthermore, in Experiment No. 6, the tensile strength after hot stamping was not measured. However, Experiment No. 6 had the same chemical composition as Experiment No. 7 and similar reduction annealing conditions. Furthermore, the hot stamping heating conditions and shot blasting conditions were also nearly identical. However, since the hot stamping start temperature in Experiment No. 6 was higher than in Experiment No. 7, it is assumed that the cooling rate after hot stamping was faster than in Experiment No. 7. Therefore, it is assumed that the martensite structure formed also hardens. Furthermore, it is assumed that the strength increases by approximately 80 MPa, and the strength (approximately 1300 MPa) estimated based on the value in Experiment No. 7 is listed.

[0120] Furthermore, in Experiment No. 6, the Fe concentration in the coating layer after hot stamping was not measured. However, Experiment No. 6 had the same chemical composition as Experiment No. 7, and the reduction annealing conditions were similar, so it is assumed that the decarburized layer formed was the same. Furthermore, the hot stamp heating conditions and shot blasting conditions were also the same. However, the coating weight in Experiment No. 6 was less than in Experiment No. 7, and the Fe concentration in the coating layer is assumed to be approximately 1% higher than in Experiment No. 7. Therefore, the Fe concentration in the coating layer after hot stamping in Experiment No. 6 is assumed to be approximately 60% of the value in Experiment No. 7, and this assumed value is shown here.

[0121] In Experiment No. 7, no LME cracking evaluation was performed. However, Experiment No. 7 had the same chemical composition as Experiment No. 6, and the reduction annealing conditions were similar, so it is assumed that the decarburized layer formed was the same. Furthermore, the hot stamping heating conditions and shot blasting conditions were also the same. It is also assumed that there is no significant difference in the Fe concentration in the coating layer expected after hot stamping. Therefore, LME cracking in Experiment No. 7 is assumed to be 0, just like in Experiment No. 6, and this assumed value is listed.

[0122] In Experiment No. 8, the Fe concentration in the coating layer after hot stamping was not measured. However, if the hot stamping conditions are the same, the Fe concentration in the coating layer after hot stamping is largely determined by the coating weight (basis weight) before hot stamping and the Fe concentration in the coating layer. Here, in Experiment No. 1 (coating weight (basis weight) 120 g / m), 2 The Fe concentration in the coating layer of Experiment No. 8 was 8.8% by mass, and the Fe concentration in the coating layer was referenced. The Fe concentration in the coating layer before hot stamping in Experiment No. 8 was equivalent to that in Experiment No. 1, but the coating weight (basis weight) in Experiment No. 8 was greater than that in Experiment No. 1. Therefore, the Fe concentration in the coating layer after hot stamping in Experiment No. 8 is assumed to be lower than the value (44% by mass) measured in Experiment No. 1. Therefore, Table 8 shows a value of 44% by mass or less as the Fe concentration in the coating layer after hot stamping that is assumed for Experiment No. 8.

[0123] In Experiments No. 9 and 10, the Fe concentration in the coating layer after hot stamping was not measured. However, as described above, the Fe concentration in the coating layer after hot stamping is generally determined by the coating weight (basis weight) and the Fe concentration in the coating layer before hot stamping, assuming the same hot stamping conditions. Experiment No. 4 was used as a reference here. The Fe concentrations in the coating layers before hot stamping in Experiments No. 9 and 10 were equivalent to those in Experiment No. 4, while the coating weights (basis weights) in Experiments No. 9 and 10 were greater than those in Experiment No. 4. Therefore, the Fe concentrations in the coating layers after hot stamping in Experiments No. 9 and 10 are assumed to be lower than the value (53% by mass) measured in Experiment No. 4. Therefore, Table 8 shows the Fe concentrations in the coating layers after hot stamping assumed for Experiments No. 9 and 10 as 53% by mass or less.

[0124] In all of Experiments Nos. 1 to 3, 8 and 9, the coating weight was 45 g / m 2 As described above, the Fe concentration in the plating layer after hot stamping is 65 mass % or less, and therefore it is believed that excellent corrosion resistance is exhibited.

[0125] This application claims priority to Japanese Patent Application No. 2023-056200, filed on March 30, 2023, and Japanese Patent Application No. 2024-022727, filed on February 19, 2024. Japanese Patent Application Nos. 2023-056200 and 2024-022727 are incorporated herein by reference.

[0126] 1 Sample after welding test (welded test piece) 2 Test piece for LME crack evaluation 3 Nugget 4 Cut surface 5 Observation surface a Center part of steel plate b Edge part of steel plate Q Void R Internal crack

Claims

1. A zinc-based plated steel sheet for hot stamping, wherein the chemical composition of the base steel sheet satisfies: C: 0.15 to 0.50 mass%, Si: 0.02 to 2.5 mass%, Mn: 0.5 to 5 mass%, P: 0.03 mass% or less (including 0 mass%), S: 0.02 mass% or less (including 0 mass%), Al: 0.010 to 1 mass%, Ti: 0.005 to 0.080 mass%, and B: 0.0005 to 0.005 mass%, with the balance being Fe and unavoidable impurities, and when elemental analysis is performed by glow discharge optical emission spectrometry (GD-OES) from the surface of the plating layer in the thickness direction of the plating layer, the carbon concentration [Cf] (mass %) at a position where the concentration of Zn constituting the plating layer is 1.0 mass% and the bulk carbon concentration [Cb] (mass %) satisfy the following formula (1): [Cf]≦0.65×[Cb]...(1) 2. The zinc-based plated steel sheet for hot stamping according to claim 1, wherein the composition of the base steel sheet satisfies one or more of the following (a) and (b): (a) further comprises one or more elements selected from the group consisting of Cr: more than 0 mass% and not more than 1.2 mass%, Mo: more than 0 mass% and not more than 1 mass%, and Ca: more than 0 mass% and not more than 0.0040 mass%, (b) further comprises one or more elements selected from the group consisting of Nb: more than 0 mass% and not more than 0.040 mass%, V: more than 0 mass% and not more than 0.30 mass%, Cu: more than 0 mass% and not more than 0.30 mass%, Ni: more than 0 mass% and not more than 0.30 mass%, Mg: more than 0 mass% and not more than 0.010 mass%, and REM: more than 0 mass% and not more than 0.010 mass%.

3. A method for producing a zinc-based plated steel sheet for hot stamping, comprising an annealing step in which a hot-rolled steel sheet or a cold-rolled steel sheet satisfying the chemical composition recited in claim 1 or 2 is allowed to remain in a reducing atmosphere having a dew point of -20°C to +10°C at 500 to 930°C for 90 to 1000 seconds, and a subsequent zinc-based plating step.

4. The method for producing a zinc-based plated steel sheet for hot stamping according to claim 3, wherein the zinc-based plating process is a hot-dip galvanizing process.

Citation Information

Patent Citations

  • Steel sheet for hot forming having excellent joining strength in spot weld zone and hot formability, and hot formed article

    JP2007169679A

  • Steel sheet for hot stamp

    JP2019173158A

  • Hot stamping alloyed hot-dip galvanized steel sheet, hot stamping molding and method for manufacturing them

    JP2022131411A

  • Storage rack

    JP2023056200A

  • Thoracoscopic surgical port