Laminated piezoelectric body, touch panel, and method for manufacturing laminated piezoelectric body
By integrating a charge dispersion layer on the fluororesin-based piezoelectric film to disperse charge density and using a transparent adhesive layer with the laminated piezoelectric body, the issue of low signal strength in fluororesin-based piezoelectric sensors is resolved, enhancing sensitivity and transparency for effective pressure detection in touch panels.
Patent Information
- Application Number
- PCT/JP2024/010929
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-03
AI Technical Summary
Laminated piezoelectric bodies using fluororesin-based piezoelectric films with transparent electrodes via a transparent adhesive layer suffer from low signal strength due to localized charge polarization, leading to reduced detection sensitivity and potential noise interference.
Incorporating a charge dispersion layer on at least one surface of the piezoelectric film with a fluororesin-based piezoelectric film, which disperses and uniformizes charge density, and using a transparent adhesive layer between the piezoelectric film and the transparent electrode to enhance signal induction and sensitivity.
The solution significantly increases signal strength and detection sensitivity while maintaining transparency, enabling more accurate pressure detection in touch panels.
Smart Images

Figure JP2024010929_03102024_PF_FP_ABST
Abstract
Description
Multilayer piezoelectric element, touch panel, and method for manufacturing multilayer piezoelectric element
[0001] The present invention relates to a laminated piezoelectric body, a touch panel, and a method for manufacturing a laminated piezoelectric body.
[0002] Generally, a touch panel detects a two-dimensional position on the surface of the touch panel by touching the surface with a finger, pen, or the like. To avoid misidentification of inputs on a touch panel, it is desirable to separate selection and execution. Specifically, it is desirable to select a two-dimensional position on the touch surface and then execute the selection by applying pressure to the touch surface. Therefore, the application of pressure-sensitive sensors that detect pressure on the touch surface to touch panels has been considered.
[0003] As the pressure-sensitive sensor, the application of a piezoelectric film that generates a voltage in response to pressure has been proposed. Known piezoelectric films include those made of polymeric materials such as fluorine-based resins and polylactic acid (see, for example, Patent Documents 1 and 2).
[0004] To apply these piezoelectric films to touch panels, it is preferable to directly place indium tin oxide (ITO) as a transparent electrode on the piezoelectric film. To form a transparent electrode using ITO, an ITO film is formed on a substrate and heat-treated to increase the crystallinity of the ITO, thereby reducing the resistance of the transparent electrode and increasing its transparency. The substrate is heat-treated (annealed) at several hundred degrees for glass substrates and at 140-150°C for polyethylene terephthalate (PET) films. When an ITO film is formed on a piezoelectric film containing a fluorine-based resin, there is a problem that the color tends to change when treated at high temperatures as described above, and high transparency cannot be maintained.
[0005] In response to this, Patent Documents 3 and 4 disclose transparent piezoelectric sheets in which a piezoelectric film and a transparent electrode film are laminated via a transparent adhesive layer. Patent Document 4 states that even if a transparent electrode is disposed on a piezoelectric film via a transparent adhesive layer, not only is it possible to detect touch pressure, but also that high transparency can be maintained because an existing transparent electrode film can be used.
[0006] International Publication No. 2016 / 098597 Japanese Patent Application Laid-Open No. 2011-006596 International Publication No. 2020 / 152464 Japanese Patent Application Laid-Open No. 2011-222679
[0007] However, according to the investigations of the present inventors, as shown in Patent Document 4, when a laminated piezoelectric element in which a transparent electrode film is laminated on a piezoelectric film containing a fluorine-based resin via a transparent adhesive layer is used as a pressure-sensitive sensor, the signal strength is found to be low.
[0008] If the signal strength is low, the electrical signal generated by pressure sensing is likely to be buried in noise, resulting in a low signal-to-noise ratio, which makes it difficult to detect pressure with high sensitivity.
[0009] The present invention has been made in view of the above circumstances, and has an object to provide a laminated piezoelectric element, a touch panel, and a method for manufacturing a laminated piezoelectric element that can detect pressure with high sensitivity while maintaining transparency.
[0010] [1] A laminated piezoelectric material containing a fluorine-based resin as a main component, and having a piezoelectric constant d 33 a piezoelectric film having a surface resistivity of 7 pC / N or more and 40 pC / N or less; and a piezoelectric film having a surface resistivity of 1.0×10 4 Ω / sq. More than 1.0×10 12A laminated piezoelectric element having a charge dispersion layer having a resistivity of Ω / sq. or less, a transparent electrode, and a transparent adhesive layer disposed between the transparent electrode and the charge dispersion layer, wherein the laminated piezoelectric element has a total light transmittance of 80% or more. [2] The laminated piezoelectric element according to [1], wherein the charge dispersion layer has a thickness of 10 nm or more and 1,000 nm or less. [3] The laminated piezoelectric element according to [1] or [2], wherein the fluororesin is a polymer containing, as a main component, a structural unit derived from vinylidene fluoride. [4] The laminated piezoelectric element according to [3], wherein the fluororesin is a vinylidene fluoride homopolymer. [5] The laminated piezoelectric element according to any one of [1] to [4], wherein the transparent adhesive layer has a thickness of 10 μm or more and 100 μm or less. [6] The laminated piezoelectric element according to any one of [1] to [5], wherein the piezoelectric film has a thickness of 25 μm or more and 120 μm or less. [7] A touch panel including the laminated piezoelectric element according to any one of [1] to [6]. [8] A method for manufacturing a laminated piezoelectric body according to any one of [1] to [6], comprising the steps of preparing the piezoelectric film, applying a composition for a charge dispersion layer to at least one surface of the piezoelectric film to form the charge dispersion layer, and bonding the charge dispersion layer of the laminate and a transparent electrode via the transparent adhesive layer. [9] The method for manufacturing a laminated piezoelectric body according to [8], wherein the step of preparing the piezoelectric film includes stretching a film containing a fluorine-based resin as a main component, and then performing a polarization treatment.
[0011] According to the present invention, it is possible to provide a laminated piezoelectric element, a touch panel, and a method for manufacturing a laminated piezoelectric element that can detect pressure with high sensitivity while maintaining transparency.
[0012] 1 is a schematic cross-sectional view showing the configuration of a laminated piezoelectric element according to this embodiment, and FIG. 2 is a schematic cross-sectional view showing a laminated piezoelectric element according to a modified example.
[0013] As described above, the reason why the signal intensity of the laminated piezoelectric body in which a piezoelectric film containing a fluorine-based resin as a main component and a transparent electrode film are laminated via a transparent adhesive layer is small is presumed to be as follows.
[0014] The polarization behavior that occurs when pressure is applied varies depending on the type of resin. For example, polylactic acid has a piezoelectric constant d14 In other words, when pressure is applied perpendicular to the film surface to a piezoelectric film containing polylactic acid, the film bends, generating shear stress, which causes polarization in a direction perpendicular to the shear plane. Therefore, the polarized charge on the film surface is not limited to the pressed area of the film, but tends to occur over a relatively wide area of the film surface.
[0015] On the other hand, fluorine-based resins mainly have a piezoelectric constant d 33 The piezoelectric constant d 33 indicates that when stress is applied in three axes (z-axis direction), polarization occurs in three axes. That is, when pressure is applied to a piezoelectric film containing a fluorine-based resin in a direction perpendicular to the film surface (triaxial direction), charge polarization occurs in the perpendicular direction (triaxial direction). Therefore, charge polarization tends to occur locally in the pressed area of the film surface, resulting in a very high charge density in the pressed area. In this area, the increase in charge density in response to stress may reach a saturation point. Therefore, when the charge density is saturated, charge is not sufficiently induced in the electrode on the opposite side of the piezoelectric film via the transparent adhesive layer, and signal strength tends to be low.
[0016] Therefore, in the present invention, a charge dispersion layer is disposed on at least one surface of a piezoelectric film containing a fluorine-based resin as a main component. As a result, even if localized areas of high charge density occur in the piezoelectric film, the charge dispersion layer can disperse and uniformize the charge. This makes it possible to avoid saturation of charge density. Furthermore, even when a piezoelectric film and a transparent electrode film are laminated via a transparent adhesive layer, charge is sufficiently induced toward the transparent electrode, thereby increasing signal strength and improving detection sensitivity. Below, a laminated piezoelectric element according to one embodiment of the present invention and a method for manufacturing the same are described.
[0017] 1. Multilayer Piezoelectric Body Fig. 1 is a schematic cross-sectional view showing the configuration of a multilayer piezoelectric body 100 according to this embodiment.
[0018] As shown in FIG. 1 , the laminated piezoelectric element 100 according to this embodiment includes a piezoelectric film 110, a first charge dispersion layer 120, a second charge dispersion layer 130, a first transparent electrode film 140, a second transparent electrode film 150, a first transparent adhesive layer 160, and a second transparent adhesive layer 170.
[0019] Hereinafter, in this specification, the first charge dispersion layer 120 and the second charge dispersion layer 130 are collectively referred to as "charge dispersion layers"; the first transparent electrode film 140 and the second transparent electrode film 150 are collectively referred to as "transparent electrode films"; and the first transparent adhesive layer 160 and the second transparent adhesive layer 170 are collectively referred to as "transparent adhesive layers."
[0020] 1-1. Piezoelectric film 110 The piezoelectric film 110 contains a fluorine-based resin as a main component and has a piezoelectric constant d 33 The d of the piezoelectric film 110 is adjusted to be equal to or greater than 7 pC / N and equal to or less than 40 pC / N. 33 When the piezoelectric constant d of the piezoelectric film is 7 pC / N or more, the amount of charge generated by pressing is sufficient, and the film functions as a pressure sensor with high sensitivity. 33 When the piezoelectric constant d of the piezoelectric film is 40 pC / N or less, the unevenness of the film surface caused by the polarization treatment can be further reduced, and therefore, the appearance defect can be reduced. 33 is more preferably 10 pC / N or more and 30 pC / N or less, and further preferably 12 pC / N or more and 30 pC / N or less.
[0021] Piezoelectric constant d 33 is one of the indices that shows the polarization behavior when a certain pressure is applied. 33 The larger the σ, the greater the degree of polarization that occurs when subjected to a certain pressure, and the greater the charge density.
[0022] The piezoelectric constant d of the piezoelectric film 110 33 can be calculated by measuring the charge generated when stress is applied to the piezoelectric film in the thickness direction at a constant speed, and is calculated using the direct quasi-static method (d 33 The piezoelectric constant d of the piezoelectric ceramic measured by the Meter method and the Berlincoat method 33 Test method: Piezoelectric constant d according to ISO 19622:2018 33Specifically, a piezoelectric constant measuring device (for example, Piezometer System PM300 manufactured by PIEZOTEST) is used to clip a piezoelectric film sample with 1 N, and the generated charge is read when a force of 0.15 N and 110 Hz is applied.
[0023] The piezoelectric constant d of the piezoelectric film 110 33 can be adjusted mainly by the type of resin contained in the piezoelectric film 110 and the manufacturing conditions (conditions for polarization and stretching). For example, among fluorine-based resins, the more structural units derived from vinylidene fluoride a resin contains, the lower the piezoelectric constant d 33 In addition, by strengthening the polarization process or stretching process, the piezoelectric constant d 33 tends to become large.
[0024] As described above, the piezoelectric film 110 contains a fluororesin as a main component. "Containing a fluororesin as a main component" means that the content of resins containing fluororesin as a structural unit (including the fluororesin itself) in the total mass of the resins constituting the piezoelectric film is 50% by mass or more. The fluororesin content is preferably 60% by mass or more, and more preferably 80% by mass or more. The upper limit of the content is not particularly limited and may be 100% by mass or 90% by mass or less.
[0025] Among fluororesins, from the viewpoint that a high piezoelectric effect is easily obtained, the fluororesin is preferably a polymer containing a structural unit derived from vinylidene fluoride as a main component.
[0026] In a polymer containing vinylidene fluoride-derived structural units as a main component, the content of vinylidene fluoride-derived structural units is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more, relative to the total amount of structural units of the polymer. The higher the content, the more likely it is that a higher piezoelectric effect will be obtained. The upper limit of the content is not particularly limited and may be 100% by mass or 90% by mass or less.
[0027] The polymer may further contain a structural unit derived from a monomer copolymerizable with vinylidene fluoride, provided that the effects of the present invention are not impaired. Examples of the monomer copolymerizable with vinylidene fluoride include fluorine-containing monomers such as trifluoroethylene, tetrafluoroethylene, hexafluoropropylene, trifluorochloroethylene, and vinyl fluoride. Two or more of these monomers may be contained.
[0028] Among them, the piezoelectric constant d 33 From the viewpoint of easily increasing the capacitance and increasing the sensitivity of a pressure-sensitive sensor using the piezoelectric film, the piezoelectric film is preferably a vinylidene fluoride homopolymer.
[0029] The thickness of the piezoelectric film 110 is preferably, for example, 25 μm or more and 120 μm or less. When the thickness of the piezoelectric film is 25 μm or more, the amount of charge generated by the piezoelectric effect increases, making it easier to increase signal strength. The thickness of the piezoelectric film is more preferably 30 μm or more, and even more preferably 35 μm or more. When the thickness of the piezoelectric film is 120 μm or less, the transparency of the piezoelectric film is less likely to be impaired, and 100 μm or less is more preferable, and 80 μm or less is even more preferable. From the same perspective, the thickness of the piezoelectric film is more preferably 35 μm or more and 80 μm or less.
[0030] 1-2. First Charge Dispersion Layer 120, Second Charge Dispersion Layer 130 (First Charge Dispersion Layer 120) The first charge dispersion layer 120 is disposed on one surface of the piezoelectric film. The first charge dispersion layer 120 increases the mobility within the charge dispersion layer of polarization charges that are locally generated by pressure on one surface of the piezoelectric film 110. This makes it possible to reduce saturation and counting losses that occur when detecting polarization charges, thereby improving the sensitivity of the piezoelectric sensor.
[0031] The first charge dispersion layer 120 has electrical conductivity. One indicator of electrical conductivity is surface resistivity. The surface resistivity of the first charge dispersion layer 120 is 1.0×10 4 Ω / sq. More than 1.0×10 12 The surface resistivity is 1.0×10 Ω / sq. or less. 12When the surface resistivity is 1.0×10 Ω / sq. or less, the first charge dispersion layer 120 has sufficient conductivity, so that the charge generated at the pressed portion of the piezoelectric film 110 by pressing easily moves within the charge dispersion layer, and when detecting the polarization charge, it becomes possible to detect it as a signal without saturation or counting losses. As a result, the signal strength can be increased even in a laminated piezoelectric element having a transparent adhesive layer. On the other hand, when the surface resistivity is 1.0×10 Ω / sq. or less, the first charge dispersion layer 120 has sufficient conductivity, so that the charge generated at the pressed portion of the piezoelectric film 110 by pressing easily moves within the charge dispersion layer, and when detecting the polarization charge, it becomes possible to detect it as a signal without saturation or counting losses. 4 When the surface resistivity is 1.0×10 Ω / sq. or more, the transparency of the first charge dispersion layer 120 is less likely to be impaired. 4 Ω / sq or more 1.0×10 9 Ω / sq or less is more preferable, and 1.0 × 10 6 Ω / sq or more 1.0×10 9 The surface resistivity can be measured in accordance with JIS K 6911 using a known resistivity meter, for example.
[0032] The surface resistivity can be adjusted by the thickness of the first charge dispersion layer 120 and the type and content of the conductive polymer or conductive material contained in the first charge dispersion layer 120. For example, increasing the thickness of the first charge dispersion layer 120 reduces the surface resistivity. Furthermore, increasing the content of the conductive polymer or conductive material in the first charge dispersion layer 120 reduces the surface resistivity.
[0033] The first charge dispersion layer 120 may be configured so that its surface resistivity falls within the above range. The first charge dispersion layer 120 includes a conductive polymer or a conductive material other than a conductive polymer. In this embodiment, the first charge dispersion layer 120 may include a cured product of a curable composition including a conductive polymer or a conductive material other than a conductive polymer, a polymerizable compound, and an optional curing agent.
[0034] Examples of the conductive polymer include polyacetylene or a derivative thereof, polythiophene or a derivative thereof, polypyrrole or a derivative thereof, polyaniline or a derivative thereof, polyphenylene or a derivative thereof, polyphenylene vinylene or a derivative thereof, polynaphthalene or a derivative thereof, polyacene or a derivative thereof, etc. Among these, polythiophene or a derivative thereof is preferred from the viewpoint of high transparency and high conductivity.
[0035] Examples of conductive materials include carbon nanotubes and graphene.
[0036] The polymerizable compound may be a thermally polymerizable compound or a photopolymerizable compound, and examples thereof include acrylic compounds, epoxy compounds, oxetane compounds, polyurethane compounds, polyimide resins, melamine resins, silicone compounds, and vinyl acetate.
[0037] The thickness of the first charge dispersion layer 120 may be within a range sufficient to disperse the charge generated in the piezoelectric film 110, preferably 10 nm to 1000 nm. A thickness of 10 nm or greater facilitates the movement of the polarization charge generated on the surface of the piezoelectric film 110 within the charge dispersion layer, thereby reducing saturation and counting losses that occur during polarization charge detection, and thus further increasing signal strength. A thickness of 1000 nm or less reduces coloring due to conductive polymers and poor appearance due to surface irregularities of the piezoelectric film 110, and thus reduces the loss of transparency. From the same perspective, the thickness of the first charge dispersion layer 120 is more preferably 20 nm to 800 nm, even more preferably 30 nm to 600 nm, and particularly preferably 40 nm to 400 nm.
[0038] (Second Charge Dispersion Layer 130) The second charge dispersion layer 130 is disposed on the other surface of the piezoelectric film 110. The piezoelectric constant d 33 In the piezoelectric film described above, charges are polarized on both surfaces of the piezoelectric film when pressed. Therefore, it is preferable to provide charge dispersion layers on both surfaces of the piezoelectric film. Similarly to the above, the second charge dispersion layer 130 is provided on the other surface of the piezoelectric film on which the first charge dispersion layer is provided. This increases the mobility of the polarization charges locally generated by pressure within the charge dispersion layer, thereby reducing saturation and count losses that occur when detecting the polarization charges and improving the sensitivity of the piezoelectric sensor.
[0039] In this embodiment, the second charge dispersion layer 130 has the same or similar configuration as the first charge dispersion layer 120, and therefore a detailed description thereof will be omitted. That is, the configuration, materials, physical properties, etc. of the second charge dispersion layer 130 are the same as the configuration, materials, physical properties, etc. of the first charge dispersion layer 120.
[0040] The composition of the first charge dispersion layer 120 and the composition of the second charge dispersion layer 130 may be the same or different. Furthermore, the thickness of the first charge dispersion layer 120 and the thickness of the second charge dispersion layer 130 may be the same or different.
[0041] 1-3. First Transparent Electrode Film 140, Second Transparent Electrode Film 150 (First Transparent Electrode Film 140) The first transparent electrode film 140 is disposed on the first charge dispersion layer 120 side of the piezoelectric film 110. The first transparent electrode film 140 includes a base layer 141 and a first transparent electrode 142; the first transparent electrode 142 detects the charges generated in the piezoelectric film 110 as an electrical signal via the first charge dispersion layer 120.
[0042] The base layer 141 is a transparent resin layer for supporting the first transparent electrode 142. The transparent resin contained in the base layer 141 is preferably a heat-resistant material that can withstand the heat required to crystallize ITO or the like. Examples of such transparent resins include polyesters such as polyethylene terephthalate (PET). Of these, PET is preferred.
[0043] The thickness of the base layer 141 is not particularly limited as long as it can support the first transparent electrode 142, but is preferably 2 μm or more and 300 μm or less, more preferably 10 μm or more and 200 μm or less, even more preferably 20 μm or more and 150 μm or less, and particularly preferably 30 μm or more and 130 μm or less.
[0044] The first transparent electrode 142 is disposed on the surface of the base layer 141 facing the first charge dispersion layer 120. The first transparent electrode 142 is preferably an inorganic electrode such as ITO (indium tin oxide) or tin oxide, and more preferably ITO.
[0045] (Second Transparent Electrode Film 150) The second transparent electrode film 150 is disposed on the second charge dispersion layer 130 side of the piezoelectric film 110. The second transparent electrode film 150 includes a base layer 151 and a second transparent electrode 152; the second transparent electrode 152 extracts the charges generated in the piezoelectric film 110 as an electrical signal via the second charge dispersion layer 130.
[0046] In this embodiment, the second transparent electrode film 150 has the same configuration as the above-described first transparent electrode film 140. That is, the configuration, material, and physical properties of the second transparent electrode film 150 may be the same as the configuration, material, and physical properties of the above-described first transparent electrode film 140.
[0047] The composition of the first transparent electrode 142 constituting the first transparent electrode film 140 and the composition of the second transparent electrode 152 constituting the second transparent electrode film 150 may be the same as or different from each other.
[0048] 1-4. First Transparent Adhesive Layer 160, Second Transparent Adhesive Layer 170 (First Transparent Adhesive Layer 160) The first transparent adhesive layer 160 is disposed between the first charge dispersion layer 120 and the first transparent electrode 142, and bonds the piezoelectric film 110 on which the first charge dispersion layer 120 is disposed to the first transparent electrode 142.
[0049] The first transparent adhesive layer 160 is preferably transparent and has enough elasticity to transmit a pressing force to the piezoelectric film 110. Examples of adhesives contained in the first transparent adhesive layer 160 include acrylic adhesives, rubber adhesives, silicone adhesives, polyester adhesives, polyurethane adhesives, polyamide adhesives, epoxy adhesives, vinyl alkyl ether adhesives, and fluorine adhesives. Among these, acrylic adhesives are preferred from the viewpoints of adhesion and elasticity.
[0050] The thickness of the first transparent adhesive layer 160 is not particularly limited, but is preferably 10 μm to 100 μm, more preferably 15 μm to 80 μm, and even more preferably 20 μm to 60 μm. When the thickness of the first transparent adhesive layer is 10 μm or more, the first charge dispersion layer 120 and the first transparent electrode 142 are more easily adhered to each other. When the thickness of the first transparent adhesive layer 160 is 100 μm or less, preferably 60 μm or less, a larger amount of charge is extracted from the first charge dispersion layer 120, making it easier to increase signal strength.
[0051] (Second Transparent Adhesive Layer 170) The second transparent adhesive layer 170 is disposed between the second charge dispersion layer 130 and the second transparent electrode 152, and bonds the piezoelectric film 110 on which the second charge dispersion layer 130 is disposed to the second transparent electrode 152. The adhesive contained in the second transparent adhesive layer 170 is the same as the adhesive contained in the first transparent adhesive layer 160 described above. The adhesive contained in the second transparent adhesive layer 170 and the adhesive contained in the first transparent adhesive layer 160 may be the same or different.
[0052] 1-5. Other Layers The laminated piezoelectric body 100 may further include layers other than those described above, as long as the effects of the present invention are not impaired. For example, a hard coat layer may be further disposed between the first charge dispersion layer 120 and the first transparent adhesive layer 160, or between the second charge dispersion layer 130 and the second transparent adhesive layer 170.
[0053] The thickness of each layer constituting the laminated piezoelectric element 100 can be determined by measuring three or more points at 5 mm intervals in an area including the center of the surface of the laminated piezoelectric element 100 using a spectral interference film thickness meter (e.g., "Optical NanoGauge C13027-11" manufactured by Hamamatsu Photonics K.K.) and calculating the arithmetic mean value of the measurements. The refractive index of each layer can be measured using the method described in JIS K7142, and the refractive index can be set by identifying the main material constituting each layer. For example, the refractive index of a piezoelectric film containing PVDF can be set to 1.42, and the refractive index of the first charge dispersion layer 120 and the second charge dispersion layer 130 can be set to 1.50.
[0054] 1-6. Physical Properties The laminated piezoelectric body 100 has high transparency. The total light transmittance of the laminated piezoelectric body 100 is preferably, for example, 80% or more. The total light transmittance of the laminated piezoelectric body 100 can be measured using a haze meter (for example, NDH7000SP II manufactured by Nippon Denshoku Industries Co., Ltd.) based on the method described in JIS K 7361-1.
[0055] In the laminated piezoelectric element 100 according to the above embodiment, as described above, when pressure is applied in directions perpendicular to the surface of the piezoelectric film 110 (in the triaxial directions), polarization occurs in the triaxial directions, and the piezoelectric effect is exerted. This induces polarized charges on the surface of the piezoelectric film 110, and a distribution of charge density occurs on the surface of the piezoelectric film 110 due to the pressure distribution of the pressure.
[0056] In this embodiment, the surface of the piezoelectric film 110 has a first charge dispersion layer 120 and a second charge dispersion layer 130. This eliminates the distribution of charge density locally generated on the surface of the piezoelectric film 110 and makes it uniform. This allows pressure to be detected with high sensitivity, and when used as a pressure sensor for a touch panel, it has high detection sensitivity for depression operations.
[0057] 2. Manufacturing Method of Laminated Piezoelectric Body The laminated piezoelectric body according to this embodiment can be manufactured through the steps of (1) preparing a laminate including a piezoelectric film and a charge dispersion layer, and (2) bonding the charge dispersion layer of the prepared laminate to the transparent electrode of the transparent electrode film via a transparent adhesive layer. Note that the piezoelectric film, charge dispersion layer, transparent adhesive layer, and transparent electrode film are the piezoelectric film, charge dispersion layer, transparent adhesive layer, and transparent electrode film described above, respectively.
[0058] (1) Regarding the process of preparing the laminate: The laminate can be obtained through the steps of (1-1) obtaining a piezoelectric film containing a fluorine-based resin, and (1-2) forming a charge dispersion layer on at least one surface of the obtained piezoelectric film.
[0059] (1-1) Process for Producing Piezoelectric Film The piezoelectric film can be obtained through a process of polarizing a film containing a fluororesin. The film containing a fluororesin may be a stretched film or an unstretched film. In this embodiment, from the viewpoint of exhibiting a high piezoelectric effect, it is preferable to polarize the film containing a fluororesin after stretching it.
[0060] A film containing a fluororesin can be produced by any method, such as a melt extrusion method or a solution casting method. Among these, a film containing a fluororesin is preferably produced by a melt extrusion method. In the melt extrusion method, a fluororesin and any additives are heated and melted in the cylinder of an extruder, and then extruded through a die to obtain a film.
[0061] The obtained film has a structure in which α-type crystals (main chain has a helical structure) and β-type crystals (main chain has a planar zigzag structure) are mixed. β-type crystals have a large polarization structure. Stretching the film can convert the α-type crystals into β-type crystals, and the stretching process may be performed as needed to convert the fluororesin into β-type crystals.
[0062] The stretching method is not particularly limited, and can be a known stretching method such as a tenter method or a drum method.
[0063] The stretching ratio is, for example, 3.0 times or more and 6.0 times or less. When the stretching ratio is 3.0 times or more, not only is it easy to adjust the thickness and strength of the film within an appropriate range, but polarization is also more likely to occur. When the stretching ratio is 3.0 times or more, the rearrangement reaction of the β-type crystals proceeds sufficiently, making it easy to exhibit higher piezoelectricity and further increasing transparency. When the stretching ratio is 6.0 times or less, breakage due to stretching can be further suppressed.
[0064] The resulting stretched film is subjected to a polarization treatment. The polarization treatment can be performed, for example, by applying a DC voltage between a ground electrode and a needle-like electrode. The voltage may be adjusted depending on the thickness of the stretched film, and may be, for example, 1 kV to 50 kV.
[0065] In this embodiment, as described above, a piezoelectric film can be obtained by polarizing a stretched film.
[0066] (1-2) Step of forming charge dispersion layer A curable composition containing, for example, the above-mentioned conductive polymer or conductive material is applied to the surface of the obtained piezoelectric film, and then dried and cured to form a charge dispersion layer.
[0067] The composition may further contain water and a solvent in addition to the above components. Examples of the solvent include alcohol solvents such as methanol, ethanol, and isopropyl alcohol.
[0068] The coating method is not particularly limited, and may be any of spin coating, gravure coating, die coating, bar coating, dip coating, and the like.
[0069] The composition can be dried by heating the applied composition. The heating temperature is preferably a temperature at which the solvent can be removed or higher and a temperature at which the fluorine-based resin constituting the piezoelectric film is heated or lower than the heat distortion temperature, and can be, for example, 100°C or higher and 150°C or lower. The heat distortion temperature can be measured, for example, in accordance with JIS K 7191-2:2015. The composition can be cured by photocuring or heat curing. When heat curing is performed, drying and heat curing can be performed simultaneously.
[0070] (2) Bonding Step The charge dispersion layer of the laminate and the transparent electrode film are bonded together via a transparent adhesive layer.
[0071] The lamination method is not particularly limited, but may be performed by laminating a transparent adhesive layer onto the charge dispersion layer of the laminate, and then laminating the transparent adhesive layer and the transparent electrode film together, with the transparent electrode of the transparent electrode film facing the transparent adhesive layer.
[0072] The laminated piezoelectric element according to this embodiment can be used for various purposes. In particular, since the laminated piezoelectric element according to this embodiment has high transparency and can detect pressure with high sensitivity, it can be preferably used as a pressure-sensitive sensor for touch panels mounted on various electronic devices.
[0073] 3. Modifications Although in the above embodiment the charge dispersion layer is disposed on both sides of the piezoelectric film, it may be disposed on only one side.
[0074] 2 is a schematic cross-sectional view showing a modified laminated piezoelectric element 100. As shown in FIG. 2, the modified laminated piezoelectric element 100 can have the same configuration as the above embodiment except that the second charge dispersion layer 130 is omitted. When the laminated piezoelectric element 100 further includes another layer, the other layer may be further included between the piezoelectric film 110 and the second transparent electrode 152.
[0075] The present invention will be further described below with reference to examples and comparative examples, but the technical scope of the present invention is not limited thereto.
[0076] 1. Evaluation of Physical Properties (1) Thickness of Charge Dispersion Layer The thickness of the charge dispersion layer formed on the piezoelectric film was measured using a spectroscopic interference film thickness meter ("Optical NanoGauge C13027-11" manufactured by Hamamatsu Photonics K.K.). Specifically, the thickness of the charge dispersion layer on the piezoelectric film, including the center of the surface, was measured at 30 points at 5 mm intervals, and the arithmetic mean value was calculated. The refractive index of each layer was set for each material, and was set to 1.42 for the piezoelectric film containing PVDF and 1.50 for the charge dispersion layer.
[0077] (2) Surface Resistivity A sample film was obtained by cutting a piezoelectric film having a charge dispersion layer to a size of 100 mm x 100 mm. The surface resistivity of the charge dispersion layer of the sample film was measured using a surface resistance meter F-109 (manufactured by Hozan Corporation) in accordance with JIS 6911. The measurement was performed at an output of 100 W, and the value was read after 10 seconds.
[0078] (3) Piezoelectric constant (piezoelectric constant d 33 ) direct quasi-static method (d 33 The piezoelectric constant d of the piezoelectric ceramic measured by the Meter method and the Berlincoat method 33 Test method: According to ISO 19622:2018, the piezoelectric constant d 33 Specifically, the piezoelectric constant d 33The sample was clipped with 1 N and a force of 0.15 N, 110 Hz was applied using a piezoelectric constant measuring device ("Piezometer System PM300", manufactured by PIEZOTEST Co., Ltd.), and the generated charge was read. 33 The measured values are measured at a temperature of 25° C. and may be positive or negative depending on whether the film is measured on the front or back, but absolute values are shown in this specification.
[0079] (piezoelectric constant d 14 Al was vapor-deposited on both sides of the piezoelectric film, and the film was cut into a 120 mm x 10 mm rectangular piece at a 45° angle to the stretching direction (MD) of the piezoelectric film and a 10 mm rectangular piece at a 45° angle to the MD direction. This was used as the measurement sample. The sample was then placed in a tensile tester with a 70 mm inter-chuck distance to prevent slack. A force was then applied to the sample at a rate of 5 mm / min, oscillating between 4 N and 9 N. To measure the amount of charge generated in the sample in response to the applied force, a capacitor with a capacitance of Qm (F) was connected in parallel to the sample, and the terminal voltage Vm of this capacitor Cm (95 nF) was measured via a buffer amplifier. The generated charge Q (C) was calculated as the product of the capacitor capacitance Cm and the terminal voltage Vm. The piezoelectric constant d 14 was calculated using the following formula: 14 = (2 x t) / L x Cm ΔVm / ΔF t: sample thickness (m) L: distance between chucks (m) Cm: capacitance of parallel-connected capacitors (F) ΔVm / ΔF: ratio of voltage change between capacitor terminals to change in force
[0080] 2. Preparation and Evaluation of Laminated Piezoelectric Body [Example 1] (1) Preparation of Piezoelectric Film A polyvinylidene fluoride film (Kureha Corporation, a film containing 100% by mass of vinylidene fluoride homopolymer) was stretched in the MD direction at a stretch ratio of 4.2 times, and then a DC voltage was applied between a ground electrode and a needle-shaped electrode while increasing from 0 kV to 11.0 kV, thereby performing a polarization treatment, and a piezoelectric film having a thickness of 42 μm was obtained.
[0081] (2) Formation of Charge Dispersion Layer A solution obtained by mixing liquid A of paint P-400MP-A (manufactured by Nagase ChemteX Corporation), which contains PEDOT:PSS as a conductive polymer, and liquid B of paint P-400MP-B (manufactured by Nagase ChemteX Corporation) in a blending ratio of 4:1 was applied to surface A of the obtained piezoelectric film using a gravure coater (multi-coater manufactured by Hirano Tecseed Co., Ltd.), and heat treatment was carried out at 130°C for 1 minute to form a charge dispersion layer with a thickness of 50 nm.
[0082] (3) Formation of Transparent Adhesive Layer Next, an optical clear adhesive (OCA) sheet (Nitto Denko Corporation, CS9862UA, thickness 50 μm) was attached to the charge dispersion layer formed on surface A of the piezoelectric film and to surface B of the piezoelectric film.
[0083] (4) Preparation of Transparent Electrode Film Next, a transparent electrode precursor film (Tetlite TCF KH100NMH3-100-U8, manufactured by Oike Kogyo Co., Ltd.) prepared by sputtering indium tin oxide (ITO) on a polyethylene terephthalate (PET) film was crystallized at 150°C for 90 minutes to prepare a transparent electrode film.
[0084] (5) Fabrication of a laminated piezoelectric element Then, the ITO surface of a transparent electrode film was attached to each of the OCA sheets attached to the charge dispersion layer on the surface A of the piezoelectric film and the OCA sheet attached to the surface B. A 1.1 mm thick glass sheet was further attached to the transparent electrode film on the surface A of the piezoelectric film to fabricate a laminated piezoelectric element.
[0085] Example 2 A laminated piezoelectric body was obtained in the same manner as in Example 1, except that the thickness of the charge dispersion layer was set to 130 nm.
[0086] Example 3 A charge dispersion layer having a thickness of 50 nm was formed on the surface A of a piezoelectric film in the same manner as in Example 1. Thereafter, a paint MT-3 (Arakawa Chemical Industries, Ltd.) containing PEDOT:PSS was applied to the surface B of the piezoelectric film, dried at 80°C, and then irradiated with 400 mJ / cm using a UV irradiation device (CSOT-40 manufactured by GS Yuasa Corporation). 2The ultraviolet light was irradiated with an integrated light amount of 10 ...
[0087] An OCA sheet was then attached to each of the charge dispersion layers on the A and B sides of the piezoelectric film, and a transparent electrode film was then attached to each OCA sheet. A 1.1 mm thick glass sheet was then attached to the transparent electrode film on the A side of the piezoelectric film to obtain a laminated piezoelectric element.
[0088] Example 4 A laminated piezoelectric body was obtained in the same manner as in Example 1, except that the thickness of the OCA sheet was set to 25 μm.
[0089] Example 5 A laminated piezoelectric body was obtained in the same manner as in Example 1, except that coating liquid A was changed to paint C-169PF-A (Nagase ChemteX Corporation) containing single-walled carbon nanotubes, coating liquid B was changed to paint C-169PF-B (Nagase ChemteX Corporation), and the blending ratio of liquid A to liquid B was changed to 3:2.
[0090] Comparative Example 1 A laminated piezoelectric body was obtained in the same manner as in Example 1, except that the charge dispersion layer was not formed.
[0091] Comparative Example 2 (1) Preparation of Piezoelectric Film To 100 parts by mass of polylactic acid (product name: Ingeo™ biopolymer) manufactured by NatureWorks LLC, 1.0 part by mass of a stabilizer (a mixture of Stabaxol P400 (10 parts by mass) manufactured by Rhein Chemie, Stabaxol I (70 parts by mass) manufactured by Rhein Chemie, and Carbodilite LA-1 (20 parts by mass) manufactured by Nisshinbo Chemical Inc.) was added and dry-blended to prepare a raw material. This raw material was placed in the hopper of an extrusion molding machine, extruded through a T-die while heated to 210°C, and brought into contact with a casting roll at 50°C to form a pre-crystallized film with a thickness of 150 μm. The pre-crystallized film was uniaxially stretched in the MD direction to 3.5 times its original size at 70°C using a roll-to-roll method to obtain a uniaxially stretched film. The film had a thickness of 49.2 μm. Next, the uniaxially stretched film was annealed by contacting it with a roll at 145° C. for 15 seconds in a roll-to-roll manner, and then rapidly cooled to produce a polylactic acid-based piezoelectric film.
[0092] (2) Formation of Antistatic Hard Coat Layer An antistatic hard coat coating (Sepulgida (registered trademark) HC-A, manufactured by Shin-Etsu Polymer) was applied to one side of the obtained piezoelectric film with an applicator, dried at 60°C for 5 minutes, and then irradiated with a metal halide lamp with an integrated light intensity of 1000 mJ / cm. 2 An antistatic hard coat layer was formed on one side of the piezoelectric film by irradiating the film with ultraviolet light of 1000 kJ / cm.
[0093] (3) Fabrication of a laminated piezoelectric body An OCA sheet was attached to each of the film surface and the antistatic hard coat layer surface of the obtained piezoelectric film, and then a transparent electrode film was attached thereto in the same manner as in Example 1. A glass sheet having a thickness of 1.1 mm was further attached to the transparent electrode film on the A-side of the piezoelectric film to obtain a laminated piezoelectric body.
[0094] [Evaluation] The total light transmittance and pressure signal of the laminated piezoelectric bodies of Examples 1 to 5 and Comparative Examples 1 and 2 were evaluated by the following methods.
[0095] (Total Light Transmittance) The total light transmittance of each of the laminated piezoelectric bodies of the examples and comparative examples was measured using a haze meter ("NDH7000SP II", manufactured by Nippon Denshoku Industries Co., Ltd.) based on the method described in JIS K 7361-1.
[0096] (Detection of Pressing Signal) A laminated piezoelectric element measuring 171.7 mm in length and 233.5 mm in width was placed in a touch panel linearity evaluation system (manufactured by Japan Novel Corporation) so that the stretching direction of the piezoelectric film was uniaxial and the thickness direction was triaxial. The center of the glass surface of the laminated piezoelectric element was pressed with a force of 8 N using a robot pressing terminal (tip diameter 3 mm) from three axial directions, and the signal strength obtained at that time was measured.
[0097] To detect the pressure signal, positive and negative lead wires were drawn from the terminals of the ITO electrodes of the laminated piezoelectric body and connected to an amplifier. The voltage signal amplified by the amplifier was then converted into a digital signal via an AD converter and a filtering circuit, and the resulting digital signal was integrated to calculate the strength of the piezoelectric signal.
[0098] The configurations and evaluation results of the laminated piezoelectric bodies of Examples 1 to 5 and Comparative Examples 1 and 2 are shown in Table 1.
[0099]
[0100] As shown in Table 1, the laminated piezoelectric element of Comparative Example 1, in which a charge dispersion layer was not provided on the piezoelectric film containing a fluorine-based resin, exhibited low signal strength. Also, the laminated piezoelectric element of Comparative Example 2, in which a piezoelectric film containing polylactic acid was used, exhibited low signal strength despite the provision of a charge dispersion layer.
[0101] In contrast, it can be seen that Examples 1 to 5, in which a charge dispersion layer was provided on at least one surface of a piezoelectric film containing a fluorine-based resin, all maintained high transparency while providing high signal strength.
[0102] In particular, it is clear that the signal strength can be further increased by providing charge dispersion layers on both sides of the piezoelectric film containing a fluorine-based resin (comparison between Examples 1 and 3).
[0103] It is also clear that the signal strength can be further increased by reducing the thickness of the transparent adhesive layer (comparison between Examples 1 and 4).
[0104] The surface resistance of the charge dispersion layer was 7.1×10 6 It can be seen that by setting the resistance to Ω, the signal strength can be further increased (comparison between Examples 1 and 5).
[0105] This application claims priority based on Japanese Patent Application No. 2023-48026, filed March 24, 2023. The contents of the specification and drawings of that application are incorporated herein by reference in their entirety.
[0106] According to the present invention, it is possible to provide a laminated piezoelectric material and a touch panel that can detect pressure with high sensitivity while maintaining transparency. Therefore, the laminated piezoelectric material is suitable as a pressure-sensitive sensor for a touch panel.
[0107] REFERENCE SIGNS LIST 100 laminated piezoelectric body 110 piezoelectric film 120 first charge dispersion layer 130 second charge dispersion layer 140 first transparent electrode film 150 second transparent electrode film 160 first transparent adhesive layer 170 second transparent adhesive layer
Claims
1. A laminated piezoelectric material containing fluorine-based resin as a main component and having a piezoelectric constant d 33 a piezoelectric film having a surface resistivity of 7 pC / N or more and 40 pC / N or less; 4 Ω / sq. More than 1.0×10 12 3. A laminated piezoelectric body comprising: a charge dispersion layer having a resistance of 0.1 Ω / sq. or less, a transparent electrode, and a transparent adhesive layer disposed between said transparent electrode and said charge dispersion layer, wherein said laminated piezoelectric body has a total light transmittance of 80% or more.
2. The laminated piezoelectric element according to claim 1, wherein the charge dispersion layer has a thickness of 10 nm or more and 1000 nm or less.
3. The laminated piezoelectric element according to claim 1, wherein the fluororesin is a polymer containing, as a main component, a structural unit derived from vinylidene fluoride.
4. The laminated piezoelectric element according to claim 3, wherein the fluororesin is a vinylidene fluoride homopolymer.
5. The laminated piezoelectric element according to claim 1, wherein the transparent adhesive layer has a thickness of 10 μm or more and 100 μm or less.
6. The laminated piezoelectric element according to claim 1, wherein the thickness of the piezoelectric film is 25 μm or more and 120 μm or less.
7. A touch panel comprising the laminated piezoelectric element according to any one of claims 1 to 6.
8. A method for producing a laminated piezoelectric element according to claim 1, comprising the steps of: preparing the piezoelectric film; applying a composition for a charge dispersion layer onto at least one surface of the piezoelectric film to form the charge dispersion layer; and bonding the charge dispersion layer and the transparent electrode together via a transparent adhesive layer.
9. The method for producing a laminated piezoelectric element according to claim 8, wherein in the step of preparing the piezoelectric film, a film containing a fluorine-based resin as a main component is stretched and then polarized.
Citation Information
Patent Citations
Polymer composition and polymer piezoelectric film
JP2011006596A
Transparent piezoelectric sheet
JP2011222679A
Information processing apparatus, information processing method, and information processing program
JP2023048026A
Touch panel
WO2020152464A2
Laminated body
WO2016098597A1