Laminated polyester film and producing method thereof, and laminate
A laminated polyester film with a conductive resin layer maintains antistatic properties through controlled resistivity ranges, addressing issues of abrasion, voltage, and heating, ensuring durability and quality in display and electronic components.
Patent Information
- Application Number
- JP2024028294
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-02-28
- Publication Date
- 2024-10-11
AI Technical Summary
Existing laminated polyester films suffer from impaired antistatic properties due to abrasion, voltage application, and heating, leading to issues such as discharge marks, scratches, and reduced conductivity during long-distance transportation and multiple treatment steps.
A laminated polyester film with a resin layer containing a conductive component, such as carbon nanotubes, and specific functional groups, which maintains surface resistivity within certain ranges (R1, R2, R3) to ensure durability and antistatic performance even after heating and handling.
The film maintains consistent antistatic properties, preventing discharge and scratches, ensuring high quality and yield in applications like display and electronic components.
Smart Images

Figure 2024144169000001 
Figure 2024144169000002 
Figure 2024144169000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminated polyester film, a method for producing the same, and a laminate. [Background technology]
[0002] Thermoplastic resin films, especially polyester films, have excellent mechanical properties, electrical properties, dimensional stability, transparency, and chemical resistance, and are therefore used in the manufacturing of a wide range of components, including display components, electronic components, and battery components, in processing steps such as coating, deposition, lamination, heating, hydrophilic treatment, and peeling. However, polyester films, which are insulating polymeric materials, have drawbacks, such as the generation of discharge marks, scratches due to sticking of the film surface, and the adsorption of foreign matter such as dust, due to the static electricity generated during travel and transportation.
[0003] In order to overcome these drawbacks, antistatic films in which antistatic properties have been imparted to polyester films have been studied. Antistatic properties can be imparted, for example, by imparting electrical conductivity to the surface or inner layer of an insulating material such as a biaxially oriented polyester film, thereby neutralizing the bias of electric charge. Among these methods, the method of imparting antistatic properties by providing a conductive coating layer on the surface of a polyester film makes it easy to maintain various stable properties of the film, and various methods have been studied in the past.
[0004] As a method for imparting antistatic properties to the surface of a polyester film, for example, Patent Document 1 discloses a method in which a styrene sulfonic acid copolymer, which is an ion-conductive antistatic agent, is applied to the polyester film, while Patent Document 2 proposes a method in which an epoxy crosslinking agent is used in combination with a polythiophene-based conductive agent, which is an electron-conductive antistatic agent, to achieve both transparency and antistatic properties in the coating film.
[0005] Furthermore, in recent years, there has been research into the use of carbon nanotubes, which are an extremely stable conductive material, as a conductive material, and Patent Documents 3 to 5 propose antistatic films in which a coating containing carbon nanotubes is formed on a substrate such as a polyester film. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Publication No. 61-204240 [Patent Document 2] JP 2004-58648 A [Patent Document 3] International Publication No. 2009 / 41170 [Patent Document 4] JP 2021-171949 A [Patent Document 5] JP 2018-135492 A Summary of the Invention [Problem to be solved by the invention]
[0007] First, the present inventors verified the adhesion of the technologies of Patent Documents 1 to 5 to water-based coating materials, and found that the antistatic method of Patent Document 1 using an ion-conductive antistatic agent had insufficient antistatic properties and was prone to losing performance due to wear when processing was repeated. On the other hand, the antistatic method using a polythiophene-based conductive agent described in Patent Document 2 had sufficient antistatic properties at the initial evaluation stage, but tended to be easily damaged by repeated transport and to be easily degraded when heated.
[0008] Furthermore, the antistatic film using "carbon nanotubes (A), carbon nanotube dispersant (B), and binder resin (C)" in Patent Document 3 and the antistatic film using "(A) carbon nanotubes (B) sugar alcohol having 4 or more carbon atoms" in Patent Document 4 are both antistatic films manufactured by in-line coating, and it is difficult to achieve both the dispersion stability of nanotubes, which is related to the stretchability of the coating film in the manufacturing process, and the hardness of the coating film by adding a crosslinking agent, and as a result, there is a problem that the performance is easily lost due to wear. On the other hand, Patent Document 5 considers imparting wear resistance by imparting slipperiness by blending fine particles and a slip agent, but when it is assumed to pass through multiple processing steps, the slip agent and fine particles fall off, making the wear resistance characteristics insufficient, and it is difficult to apply in-line coating, which is a preferred manufacturing method described later, and sufficient durability is not obtained.
[0009] Therefore, an object of the present invention is to eliminate the above-mentioned drawbacks and to provide a laminated polyester film whose antistatic properties are not easily lost even when transported over long distances or subjected to multiple processing steps, particularly processing steps involving heating, and a method for producing the laminated polyester film. [Means for solving the problem]
[0010] In order to solve the above problems, the first laminated polyester film of the present invention and the second laminated polyester film of the present invention have the following configurations. Note that hereinafter, the first laminated polyester film of the present invention and the second laminated polyester film of the present invention may be collectively referred to as the laminated polyester film of the present invention.
[0011] The first laminated polyester film of the present invention is a laminated polyester film having a resin layer X on at least one surface of a polyester film, the resin layer X containing a conductive component A, and when the surface resistivity of the resin layer X is R1, the surface resistivity of the resin layer X after application of a voltage of 500 V for 120 seconds is R2, and the surface resistivity of the resin layer X after heating at 100°C for 24 hours is R3, the laminated polyester film has all of the following characteristics 1 to 3: Feature 1: R1 is 1.0×10 4 Ω / □ or more 1.0×10 10 It is less than Ω / □. Feature 2: The value of R2 / R1 is less than 3.0. Feature 3: The value of R3 / R1 is less than 3.0.
[0012] The second laminated polyester film of the present invention is a laminated polyester film having a resin layer X on at least one surface of the polyester film, the resin layer X containing a conductive component A, a resin having a hydroxyl group, a carboxyl group or a sulfo group in a side chain being resin b, a compound having at least one of a group of functional groups consisting of an amino group, a methylol group, a carbodiimide group and an oxazoline group being compound c, and a compound having at least one branched chain being compound d, the resin layer X further containing the resin b, the compound c, and the compound d.
[0013] The laminated polyester film of the present invention may have the following embodiments, and may be produced, for example, by the following production method. [1] A laminated polyester film having a resin layer X on at least one surface of a polyester film, the resin layer X containing a conductive component A, the surface resistivity of the resin layer X being R1, the surface resistivity of the resin layer X after application of a voltage of 500 V for 120 seconds being R2, and the surface resistivity of the resin layer X after heating at 100° C. for 24 hours being R3, the laminated polyester film has all of the following characteristics 1 to 3: Feature 1: R1 is 1.0×10 4 Ω / □ or more 1.0×10 10 It is less than Ω / □. Feature 2: The value of R2 / R1 is less than 3.0. Feature 3: The value of R3 / R1 is less than 3.0. [2] A laminated polyester film having a resin layer X on at least one surface of a polyester film, the resin layer X containing a conductive component A, a resin having a hydroxyl group, a carboxyl group or a sulfo group in a side chain being referred to as resin b, a compound having at least one functional group selected from the group consisting of an amino group, a methylol group, a carbodiimide group and an oxazoline group being referred to as compound c, and a compound having at least one branched chain being referred to as compound d, the resin layer X further containing the resin b, the compound c and the compound d. [3] The laminated polyester film according to [1], wherein R2 / R1 is less than 1.0. [4] The laminated polyester film according to any one of [1] to [3], wherein the conductive component A contains single-walled or double-walled carbon nanotubes having a diameter of 1 nm or more and 50 nm or less. [5] The laminated polyester film according to any one of [1], [3] and [4], wherein resin b is a resin having a hydroxyl group, a carboxyl group or a sulfo group in a side chain, and compound c is a compound having at least one functional group selected from the group consisting of an amino group, a methylol group, a carbodiimide group and an oxazoline group, wherein resin layer X contains resin b and compound c. [6] The laminated polyester film according to any one of [1] or [3] to [5], wherein the resin layer X contains compound d, where compound d is a compound having at least one branched chain. [7] The laminated polyester film according to any one of [1] to [6], which can be used as a base substrate for coating in a manufacturing process of at least one of a group of components consisting of display components, electronic components, and battery components. [8] A laminate having a resin layer Y, either directly or via an intermediate layer, on the side opposite to the resin layer X of the laminated polyester film according to any one of [1] to [7], wherein the resin layer Y is any one of an adhesive layer, a heat seal layer, and a release layer. [9] A method for producing the laminated polyester film according to any one of [1] to [8], comprising the steps of: step 1 of directly coating a polyester film with a coating composition containing a conductive component A, resin b, compound c, and compound d, and containing water as a main dispersion medium, where b is a resin having a hydroxyl group, a carboxyl group, or a sulfo group in a side chain; c is a compound having at least one functional group selected from a group consisting of an amino group, a methylol group, a carbodiimide group, and an oxazoline group; and d is a compound having at least one branched chain; step 2 of stretching the polyester film that has been subjected to step 1 in at least one axial direction; and step 3 of heating the polyester film that has been subjected to step 2 at a temperature of 200°C or more and 260°C or less.
[0014] Although both the first laminated polyester film of the present invention and the second laminated polyester film of the present invention can obtain the latter effect, a particularly preferred embodiment of the present invention is a laminated polyester film that satisfies both requirements at the same time, as will be described in detail later. Effect of the Invention
[0015] The present invention can provide a laminated polyester film that is resistant to loss of antistatic properties even after long-distance transportation and multiple treatment steps, particularly a treatment step involving heating, and a method for producing the laminated polyester film. When the laminated polyester film of the present invention is used in the production process of display members, electronic members, or battery members, it is possible to avoid deterioration in quality and yield, such as damage to members caused by discharge and inspection defects. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The first laminated polyester film of the present invention is a laminated polyester film having a resin layer X on at least one surface of a polyester film, the resin layer X containing a conductive component A, and when the surface resistivity of the resin layer X is R1, the surface resistivity of the resin layer X after application of a voltage of 500 V for 120 seconds is R2, and the surface resistivity of the resin layer X after heating at 100°C for 24 hours is R3, the laminated polyester film has all of the following characteristics 1 to 3: Feature 1: R1 is 1.0×10 4 Ω / □ or more 1.0×10 10 It is less than Ω / □. Feature 2: The value of R2 / R1 is less than 3.0. Feature 3: The value of R3 / R1 is less than 3.0.
[0017] The second laminated polyester film of the present invention is a laminated polyester film having a resin layer X on at least one surface of the polyester film, the resin layer X containing a conductive component A, a resin having a hydroxyl group, a carboxyl group or a sulfo group in a side chain being resin b, a compound having at least one of a group of functional groups consisting of an amino group, a methylol group, a carbodiimide group and an oxazoline group being compound c, and a compound having at least one branched chain being compound d, the resin layer X further containing the resin b, the compound c, and the compound d.
[0018] The present inventors have investigated the causes of the loss of antistatic functionality of polyester films due to repeated processing and have found that this is mainly caused by the following three factors, which led to the present invention. The details are described below.
[0019] The first factor is caused by the scraping or falling off of the functional layer with antistatic properties, and the properties are no longer expressed when the material is removed from the film. In other words, the presence of conductive components on the polyester film surface is a prerequisite for the properties to be expressed.
[0020] The second factor is the loss of conductivity due to the application of voltage. Antistatic films have the function of neutralizing charge imbalances, but it was discovered that once a localized charge imbalance, i.e., an electromotive force difference (voltage), occurs, the conductive components themselves that express the function can be damaged and the properties can deteriorate. This type of property deterioration due to voltage is often seen in conductive polymer materials, but it can also occur in areas of abnormal aggregation even with relatively stable carbon nanotubes when their dispersibility or fixation in the coating is insufficient.
[0021] The third factor is the loss of electrical conductivity due to heating. Loss of electrical conductivity due to heating does not only occur when the conductive material undergoes thermal decomposition, but also when the conductive material is not sufficiently fixed to the coating film and becomes free, or when high-temperature processing causes further cross-linking or volume expansion, resulting in the disconnection of the conductive path.
[0022] The laminated polyester film in the first aspect of the present invention, which is designed to eliminate the above three factors, has a resin layer X on at least one surface of a polyester film, the resin layer X contains a conductive component A, and when the surface resistivity of the resin layer X is R1, the surface resistivity of the resin layer X after application of a voltage of 500 V for 120 seconds is R2, and the surface resistivity of the resin layer X after heating at 100° C. for 24 hours is R3, the laminated polyester film has all of the following characteristics 1 to 3. Feature 1: R1 is 1.0×10 4 Ω / □ or more 1.0×10 10 It is less than Ω / □. Feature 2: The value of R2 / R1 is less than 3.0. Feature 3: The value of R3 / R1 is less than 3.0.
[0023] Here, feature 1 corresponds to the first factor mentioned above, feature 2 corresponds to the second factor, and feature 3 corresponds to the third factor. By incorporating all of these features, it is possible to obtain a laminated polyester film whose antistatic properties are unlikely to be lost even after long-distance transportation and multiple processing steps, especially processing steps that involve heating.
[0024] The first laminated polyester film of the present invention has a resin layer X on at least one surface thereof, the resin layer X contains a conductive component A, and the surface resistivity R1 of the resin layer X is 1.0×10 4 Ω / □ or more 1.0×10 10 Ω / □ or less, and 1.0×10 4 Ω / □ or more 1.0×10 8 It is preferable that the resistance is Ω / □ or less, and 1.0×10 5 Ω / □ or more 1.0×10 7 It is more preferable that the surface resistivity R1 of the resin layer X is 1.0×10 10 When the surface resistivity R1 of the resin layer X is more than 1.0×10 4 If the resistance is less than Ω / □, it may lead to malfunction of elements that transmit and receive electric signals in display components such as touch panels, various electronic components, and battery components.
[0025] On the other hand, in the first laminated polyester film of the present invention, the ratio R2 / R1, which is the ratio of the surface resistivity R1 of the resin layer X to the surface resistivity R2 of the resin layer X after applying a voltage of 500V for 120 seconds, must be less than 3.0, preferably less than 1.5, more preferably less than 1.0, and even more preferably less than 0.5. In particular, by having a resin layer X with a low R2 / R1, that is, a resistance value that decreases after application of a voltage, it becomes possible to stably exhibit excellent antistatic properties when conveyed over a long distance or passed through multiple processing steps. The lower limit of R2 / R1 is not particularly limited, but in consideration of the practical cost and abrasion resistance of the laminated polyester film, the lower limit is approximately 0.05. On the other hand, if R2 / R1 exceeds 3.0, the conductive component is easily damaged when the above-mentioned local charge bias occurs due to conveyance, and as a result, it becomes difficult to avoid the destruction of members due to discharge, deterioration of quality due to inspection failure, and reduction in yield. Various surface resistivities can be measured with a known ultra-high resistance / microcurrent meter, and the details of the measurement method will be described later.
[0026] Furthermore, in the first laminated polyester film of the present invention, the value of R3 / R1, which is the ratio of the surface resistivity R1 of the resin layer X to the surface resistivity R3 of the resin layer X after heating at 100°C for 24 hours, must be less than 3.0, preferably less than 1.5, and particularly preferably less than 0.6. There is no particular restriction on the lower limit of R3 / R1, but it is difficult in principle to achieve a value of less than 0.1. On the other hand, when R3 / R1 exceeds 3.0, the antistatic property is significantly reduced in the heat treatment step among the processing steps of the laminated polyester film, and as a result, it is difficult to avoid the destruction of members due to discharge, the deterioration of quality due to inspection failure, and the reduction in yield.
[0027] The method of imparting the three features of the first laminated polyester film of the present invention is not particularly limited, but they can be imparted by the composition and formation method of the resin layer X. Specifically, the surface resistivity R1 of feature 1 can be controlled by the amount and type of conductive component A, which is a component that imparts conductivity, as well as the amount and curing form of the resin component that forms the resin layer X, the coating thickness of the entire resin layer X, and the like. The surface resistivity R2 of the resin layer X after applying a voltage of 500 V for 120 seconds of feature 2 is particularly due to the type of conductive component A, the dispersion state in the resin component, and the manufacturing method of the resin layer X. The surface resistivity R3 of the resin layer X after heating at 100° C. for 24 hours of feature 3 is also influenced by the conductive component A, but can be controlled particularly by the composition and curing form of the resin component that holds the conductive component A in the resin layer X, and the temperature during curing.
[0028] The second laminated polyester film of the present invention, characterized by the above-mentioned various control methods (means for imparting three features), has a resin layer X on at least one surface of the outermost layer, and the resin layer X contains a conductive component A, and when a resin having a hydroxyl group, a carboxyl group or a sulfo group in a side chain is defined as resin b, a compound having at least one of a group of functional groups consisting of an amino group, a methylol group, a carbodiimide group and an oxazoline group is defined as compound c, and a compound having at least one branched chain is defined as compound d, the resin layer X further contains resin b, compound c, and compound d. The preferred structures and composition ratios of the various components, and the details of the manufacturing method of the laminated polyester film and the resin layer X will be described later.
[0029] Preferred embodiments of the laminated polyester film of the present invention will be described in detail below.
[0030] <Polyester film> The laminated polyester film of the present invention has a resin layer X on at least one side of a polyester substrate. Polyester is a general term for polymers in which an ester bond is the main bonding chain of the main chain, and those in which at least one type of structural unit selected from ethylene terephthalate, propylene terephthalate, ethylene-2,6-naphthalate, butylene terephthalate, propylene-2,6-naphthalate, ethylene-α,β-bis(2-chlorophenoxy)ethane-4,4'-dicarboxylate, etc. is the main structural unit can be preferably used.
[0031] Here, the main structural unit refers to a structural unit that is contained in the resin at more than 50 mol% and 100 mol% or less when all structural units constituting the resin are taken as 100 mol%. The main structural unit is preferably contained in the resin at more than 70 mol% when all structural units constituting the resin are taken as 100 mol%. The laminated polyester film refers to a sheet-like material having at least two layers and containing polyester as the main component. The main component refers to a component that is contained in the object at more than 50 mass% and 100 mass% or less of all structural components. The polyester base material refers to a sheet-like material that constitutes the laminated polyester film and contains polyester as the main component. The above polyester may contain 30 mol% or less of a copolymer component in all structural components as necessary.
[0032] As the polyester substrate in the laminated polyester film of the present invention, a polyethylene terephthalate film is preferably used from the viewpoint of heat resistance and smoothness. In addition, when heat or shrinkage stress acts on the laminated polyester film, a polyethylene-2,6-naphthalate film having excellent heat resistance and rigidity is preferably used. Here, the polyethylene terephthalate film refers to a film in which polyethylene terephthalate (including copolymers) accounts for more than 50% by mass and not more than 100% by mass of all components constituting the film, and the same can be interpreted for a polyethylene-2,6-naphthalate film.
[0033] From the viewpoint of thermal stability and mechanical strength, the polyester substrate is preferably biaxially oriented, that is, a biaxially oriented polyester film. The biaxially oriented polyester film refers to a polyester film that shows a pattern oriented along two orthogonal axes in wide-angle X-ray diffraction. In general, a biaxially oriented polyester film is obtained by stretching an unstretched polyester sheet in two orthogonal directions, for example, by stretching the polyester sheet in the longitudinal direction and the width direction by about 2.5 to 5.0 times, and then performing a heat treatment to complete crystal orientation. By using a biaxially oriented polyester film as the polyester substrate, the thermal stability, particularly the dimensional stability and mechanical strength of the laminated polyester film are improved, and the planarity is also improved. Here, the longitudinal direction refers to the direction in which the film runs during the manufacturing process (in the case of a film roll, this corresponds to the winding direction of the film), and the width direction refers to the direction perpendicular to the longitudinal direction within the film plane.
[0034] The polyester substrate may also contain various additives, such as antioxidants, heat stabilizers, weather stabilizers, UV absorbers, organic lubricants, pigments, dyes, organic or inorganic fine particles, fillers, antistatic agents, nucleating agents, etc., to the extent that they do not impair the effects of the laminated polyester film of the present invention. These components may be used alone or in combination.
[0035] The thickness of the polyester substrate is not particularly limited and is appropriately selected depending on the application and type, but is usually preferably 10 to 500 μm, more preferably 20 to 250 μm, and particularly preferably 25 to 100 μm in terms of mechanical strength, handleability, etc. The polyester substrate may be a composite film obtained by coextrusion, a film obtained by laminating the obtained films by various methods, or a single layer film.
[0036] The laminated polyester film of the present invention preferably has a total light transmittance of 85% or more, more preferably 87% or more, and particularly preferably 89% or more. The laminated polyester film having a total light transmittance of 85% or more can be suitably used for applications that require light transmission, such as display members, and has the advantage of facilitating quality inspection in electronic member applications. In addition, since the upper limit of the substantial total light transmittance of polyester films is 94%, it is preferable that the total light transmittance is 85% or more and 94% or less.
[0037] The total light transmittance of the laminated polyester film can be measured by using a measuring device conforming to JIS "Determination of haze of transparent materials" (K7136 2000 edition). Methods for making the total light transmittance of the laminated polyester film 85% or more include, for example, the above-mentioned biaxial stretching to improve the flatness, and forming a smooth coating layer on the outermost surface of the laminated polyester film to reduce the reflectance with the air layer.
[0038] Moreover, the laminated polyester film of the present invention preferably has a haze value of 2.0% or less, more preferably 1.0% or less. By setting the haze value of the laminated polyester film in the above range, the transparency is increased, and the film can be suitably used for display members and electronic members that require transparency. The lower the haze value, the more preferable it is, and although there is no particular limit to the lower limit, the lower limit is set to 0.1% from the viewpoint of feasibility. The haze value is also sometimes called "haze".
[0039] The haze value of the laminated polyester film can be measured by a method conforming to JIS "Determination of Haze of Transparent Materials" (K7136 2000 edition), and the details are shown in the Examples. In addition, as a method for making the haze value of the laminated polyester film 2.0% or less, for example, a method of reducing the reflectance at the interface with air by adjusting the surface shape and refractive index of the coating layer formed on the outermost surface of the polyester film can be mentioned.
[0040] In addition, the resin layer X of the laminated polyester film of the present invention preferably has a static friction coefficient of 0.50 or less, more preferably 0.45 or less. By setting the static friction coefficient of the laminated polyester film within the above range, the slipperiness is increased, so that scratches on the coating layer due to friction during transportation and the drop-off of the antistatic component can be suppressed. On the other hand, there is no particular restriction on the lower limit of the static friction coefficient from the viewpoint of antistatic properties, but if it is too small, there is a possibility that the film will slip when rolled, so that it is preferably 0.3 or more from the viewpoint of handling. The method for measuring the static friction coefficient will be described later.
[0041] <Biomass and recycled materials> In the laminated polyester film of the present invention, it is preferable that the polyester base material contains at least one of a biomass raw material and a recycled raw material from the viewpoint of reducing the environmental load. Here, biomass is an organic compound photosynthesized from carbon dioxide and water. When biomass is burned, it usually becomes carbon dioxide and water again, so that biomass can be used as a so-called carbon-neutral renewable energy.
[0042] When the ratio of plant-derived carbon number to the total carbon number is taken as the biomass degree, for example, in an ethylene terephthalate unit, when only the ethylene glycol component is entirely derived from a plant, the biomass degree is theoretically 20%. To increase the biomass degree beyond that, the terephthalic acid must also be derived from a plant, which increases the effect of reducing the environmental load but increases the production cost. The ethylene glycol component and the terephthalic acid component may be a combination of a petroleum-derived component and a plant-derived component. From the viewpoint of achieving an effect of reducing the environmental load, the lower limit of the biomass degree of the polyester constituting the film is preferably 5%, more preferably 10%, and even more preferably 13%. By having a biomass degree of 5% or more, the effect of reducing the environmental load can be expected. On the other hand, the upper limit of the biomass degree is preferably as high as possible when only the reduction in the environmental load is taken into consideration, and the upper limit is 100%. However, from the viewpoint of achieving both the production cost and the reduction in the environmental load of the laminated polyester film, the biomass degree is preferably 20% or less in practice.
[0043] As a known method for analyzing the presence or absence of biomass raw materials, for example, the carbon isotope method ( 14 C) is used.
[0044] The recycled raw material is a raw material obtained by recovering and decomposing polyester that has been produced as a chemical product once or several times, and reusing it. Examples of the recycled raw material for the laminated polyester film of the present invention include uncoated portions at both ends in the width direction cut and removed in the production process of the laminated polyester film of the present invention, other recovered polyester films, and further recovered polyesters that have been distributed in a form other than a film, such as PET bottles. When producing a laminated polyester film, it is preferable to use 90% by mass or less of the recycled raw material out of 100% by mass of the polyester raw material. By limiting the use of recycled raw materials to 90% by mass or less, the amount of highly crystalline polyester that has once become a chemical product is reduced, and therefore the deterioration of the thermal properties and transparency of the obtained laminated polyester film and coloring can be reduced.
[0045] <layer> In the present invention, the term "layer" refers to a portion having a finite thickness that is distinguished from an adjacent portion by having a discontinuous boundary surface in the composition of constituent elements, the shape of inclusions such as particles, and physical properties in the thickness direction from the surface of the laminate. More specifically, when the laminate is cross-sectionally observed from the surface to the thickness direction using various composition / element analysis devices (FT-IR, XPS, XRF, EDAX, SIMS, EPMA, EELS, etc.), electron microscopes (transmission type, scanning type), or optical microscopes, it refers to a portion having a finite thickness that is distinguished by a discontinuous boundary surface.
[0046] <Resin layer X> The laminated polyester film of the present invention has a resin layer X on the outermost surface on at least one side of a polyester substrate. The resin layer X is an antistatic layer that contains a preferable conductive component A described below and thereby imparts antistatic properties to the laminated polyester film.
[0047] From the above viewpoint, the resin layer X in the first laminated polyester film of the present invention has a surface resistivity R1 of 1.0×10 4 Ω / □ or more 1.0×10 10It is preferable that the following conditions are satisfied: Ω / □ or less, the value of R2 / R1 is less than 3.0, and the value of R3 / R1 is less than 3.0 (the surface resistivity of the resin layer X after applying a voltage of 500 V for 120 seconds is R2, and the surface resistivity of the resin layer X after heating at 100°C for 24 hours is R3).
[0048] From the above viewpoint, the resin layer X in the laminated polyester film of the present invention contains a conductive component A. Furthermore, the resin layer X in the second laminated polyester film of the present invention satisfies "containing resin b, compound c, and compound d (a resin having a hydroxyl group, a carboxyl group, or a sulfo group in a side chain is referred to as resin b, a compound having at least one of a group of functional groups consisting of an amino group, a methylol group, a carbodiimide group, and an oxazoline group is referred to as compound c, and a compound having at least one branched chain is referred to as compound d)." The definitions of each parameter and resin are as described above.
[0049] From the viewpoint that the resin layer X plays such a role, the laminated polyester film of the present invention has the resin layer X on at least one surface of the polyester film, and preferably has the resin layer X only on the surface of one surface. By adopting such an embodiment, when the laminated polyester film including the resin layer X is further subjected to post-processing, it becomes easy to suppress the occurrence of discharge marks due to charging, the occurrence of scratches due to sticking of the film surface, and the adsorption of foreign matter such as dust. The resin layer X can be designed in consideration of the antistatic property and its durability. The details of a preferred method for producing the resin layer X and a preferred coating composition for producing the resin layer X will be described later.
[0050] The thickness of the resin layer X (coating thickness after drying) is preferably 10 to 200 nm, more preferably 20 to 150 nm, and particularly preferably 30 to 100 nm. When the coating thickness is 10 nm or more, the above-mentioned antistatic properties can be sufficiently ensured. On the other hand, when the thickness of the resin layer X is 200 nm or less, it is easy to maintain high appearance quality such as transparency, and the amount of conductive components used can be reduced, which is advantageous in terms of cost. The thickness of the resin layer X can be measured by observing a cross section in a direction perpendicular to the film surface (thickness direction) using a transmission electron microscope (TEM). A detailed measurement method will be described later.
[0051] <Paint composition> Here, a preferred coating composition for forming the resin layer X of the laminated polyester film of the present invention will be described. The resin layer X of the second laminated polyester film of the present invention contains a conductive component A, a resin b having a hydroxyl group, a carboxyl group or a sulfo group in a side chain, a compound c having at least one of a group of functional groups consisting of an amino group, a methylol group, a carbodiimide group and an oxazoline group, and a compound d having at least one branched chain. The resin layer X in the first laminated polyester film of the present invention preferably contains the conductive component A, and further contains the resin b and the compound c or the compound d, and particularly preferably contains all of the conductive component A, the resin b, the compound c and the compound d.
[0052] Each component constituting the coating composition is such that the resin layer X formed using the coating composition satisfies the essential requirement of the first laminated polyester film of the present invention (which is also preferably satisfied in the second laminated polyester film) to "make the surface resistivity R1 of the resin layer X 1.0×10 4 Ω / □ or more 1.0×10 10 The type and content are selected so that all of the following are satisfied: R2 / R1 value is less than 3.0, and R3 / R1 value is less than 3.0.
[0053] Here, the above requirement can also be interpreted as being satisfied when a resin b having a hydroxyl group, a carboxyl group, or a sulfo group in its side chain reacts with a compound c having at least one of a group of functional groups consisting of an amino group, a methylol group, a carbodiimide group, and an oxazoline group to form a new chemical structure.
[0054] <Conductive component A> In the laminated polyester film of the present invention, it is necessary to contain a conductive component A as a component of the resin layer X. The type of conductive component A is not particularly limited, and for example, a conductive carbon material such as carbon nanotube (hereinafter, CNT), a polymer material having a conductive structure represented by a polythiophene structure, an acidic polymer in a free acid state, etc. can be used alone or in combination. In the present invention, from the viewpoint of improving the dispersibility of the conductive component A and ensuring antistatic properties and durability, it is more preferable to use a conductive carbon material, and CNT is particularly preferable.
[0055] The CNT in the present invention refers to a seamless tube in which a honeycomb-structured graphene sheet composed only of carbon atoms is rolled into a cylindrical shape. A graphene sheet wound in one layer is called a single-walled CNT, a graphene sheet wound in two layers is called a double-walled CNT, and a graphene sheet wound in three or more layers is called a multi-walled CNT. The CNT used in the present invention is preferably a straight or bent single-walled CNT, a straight or bent double-walled CNT, a straight or bent multi-walled CNT, or a combination of these. The honeycomb structure refers to a network structure mainly composed of six-membered rings, but the CNT structure may have a ring structure other than six-membered rings, such as a five-membered ring or a seven-membered ring, at the bent part of the tube or the closed part of the cross section.
[0056] Among the above CNTs, the CNTs used as the conductive component A of the laminated polyester film of the present invention are preferably straight or bent single-walled CNTs and straight and / or bent double-walled CNTs from the viewpoint of electrical conductivity. Single-walled CNTs and double-walled CNTs are excellent in terms of dispersibility in a solvent, durability, and production costs. On the other hand, multi-walled CNTs having three or more layers are excellent in dispersibility and production costs, but may not provide sufficient electrical conductivity.
[0057] In addition, the CNT used in the present invention preferably has a diameter of 1 nm or more. In addition, the diameter of the CNT is preferably 50 nm or less, more preferably 10 nm or less. When the upper diameter limit is within the above preferred range, the CNT is unlikely to have a multilayer structure of three or more layers, so that the conductive path is unlikely to diverge between layers, and the conductivity of the resin layer X can be increased. In addition, a large amount of CNT is not required, and the CNT does not fall off the resin layer X, so that a small amount can achieve sufficient antistatic properties and durability. On the other hand, CNTs having a diameter lower limit within the above preferred range are easy to manufacture and easy to obtain.
[0058] In summary, in the laminated polyester film of the present invention, the conductive component A preferably contains single-walled or double-walled CNTs having a diameter of 1 nm or more and 50 nm or less. These CNTs may be used alone or in combination.
[0059] The aspect ratio of the CNT used in the present invention is preferably 100 or more. The aspect ratio of the CNT is preferably 5,000 or less. By setting the aspect ratio of the CNT within the above range, the antistatic property of the resin layer X can be improved. When the aspect ratio of the CNT is set within the above range, when the in-line coating method described later is used in forming the resin layer X, the CNT is appropriately loosened in the stretching process, the conductive path between the CNTs is not broken, and a network with sufficient gaps between the CNTs can be formed. When such a network structure is formed, good antistatic properties can be expressed. The aspect ratio is the length (nm) of the CNT divided by the diameter (nm) of the CNT (length (nm) of the CNT / diameter (nm) of the CNT).
[0060] CNTs with such characteristics can be obtained by known manufacturing methods such as chemical vapor deposition, catalytic vapor phase growth, arc discharge, and laser evaporation. When producing CNTs, fullerenes, graphite, and amorphous carbon are simultaneously produced as by-products, and catalytic metals such as nickel, iron, cobalt, and yttrium also remain, so it is preferable to remove these impurities and purify the CNTs. To remove impurities, ultrasonic dispersion treatment is effective in addition to acid treatment with nitric acid, sulfuric acid, etc., and separation by a filter is more preferable in terms of improving purity.
[0061] Single-walled CNTs and double-walled CNTs are generally thinner than multi-walled CNTs, and if uniformly dispersed, they can secure a larger number of conductive paths per unit volume, resulting in high conductivity. However, depending on the manufacturing method, a large amount of semiconducting CNTs may be produced as a by-product, and in that case, it becomes necessary to selectively manufacture or select conductive CNTs. Multi-walled CNTs generally exhibit conductivity, but if the number of layers is too large, the number of conductive paths per unit weight decreases. Therefore, even when multi-walled CNTs are used, the CNT diameter is preferably 50 nm or less, more preferably 20 nm or less, and even more preferably 10 nm or less, as in the case of using single-walled CNTs and double-walled CNTs.
[0062] When a polythiophene compound is used as the conductive component A, for example, a compound having a structure in which the 3rd and 4th positions of the thiophene ring are substituted can be used. Furthermore, a compound in which oxygen atoms are bonded to the 3rd and 4th carbon atoms of the thiophene ring can be preferably used. When a hydrogen atom or a carbon atom is directly bonded to the carbon atom, it may not be easy to make the coating liquid water-based. The above compound can be produced by the method disclosed in, for example, JP-A-2000-6324, EP-A-602713, or U.S. Pat. No. 5,391,472, but other methods may also be used.
[0063] For example, 3,4-ethylenedioxythiophene is obtained using an alkali metal salt of 3,4-dihydroxythiophene-2,5-dicarboxy ester as a starting material, and then potassium peroxodisulfate, iron sulfate, and the previously obtained 3,4-ethylenedioxythiophene are introduced into an aqueous polystyrene sulfonic acid solution and reacted to obtain a composition in which a polythiophene such as poly(3,4-ethylenedioxythiophene) is complexed with an acidic polymer such as polystyrene sulfonic acid.
[0064] Furthermore, as an aqueous coating composition containing poly-3,4-ethylenedioxythiophene and polystyrenesulfonic acid, a composition sold under the name Baytron P by HC Starck (Germany) can be used.
[0065] On the other hand, examples of the acidic polymer in a free acid state that can be used as the conductive component A include polymeric carboxylic acid, polymeric sulfonic acid, polyvinyl sulfonic acid, etc. Examples of the polymeric carboxylic acid include polyacrylic acid, polymethacrylic acid, and polymaleic acid. Examples of the polymeric sulfonic acid include polystyrene sulfonic acid, and polystyrene sulfonic acid is particularly preferred in terms of antistatic properties. The free acid may be in the form of a partially neutralized salt. It can also be used in the form of a copolymer with other copolymerizable monomers, such as acrylic acid esters, methacrylic acid esters, and styrene.
[0066] The molecular weight of the polymeric carboxylic acid or polymeric sulfonic acid is not particularly limited, but in terms of the stability and antistatic properties of the coating material, the weight average molecular weight is preferably 1,000 to 1,000,000, more preferably 5,000 to 150,000. As long as it does not impair the characteristics of the invention, it may contain some alkali salts such as lithium salts and sodium salts, or ammonium salts. It is also considered that the salts in which the polyanions are neutralized act as dopants. This is because the equilibrium shifts to the acidic side due to the progress of the equilibrium reaction after neutralization between polystyrene sulfonic acid and ammonium salts, which function as very strong acids.
[0067] <Resin b> The resin b forming the resin layer X in the first laminated polyester film of the present invention is a resin having the above-mentioned "surface resistivity R1 of 1.0×10 4 Ω / □ or more 1.0×10 10 Any material can be used as long as it has a value of "Ω / □ or less, a value of R2 / R1 less than 3.0, and a value of R3 / R1 less than 3.0". For example, polyester resin, acrylic resin, urethane resin, epoxy resin, etc. can be used alone or in combination to satisfy the above range. On the other hand, from the viewpoint of stably expressing the antistatic property of the resin layer X by using it in combination with the conductive component A, it is particularly preferable to use an acrylic resin. Also, from the viewpoint of uniformly dispersing the conductive component A on the surface of the resin layer X by using it in combination with the conductive component A and improving the slipperiness, it is particularly preferable to use a polyester resin. Also, it is preferable to select the resin b forming the resin layer X in the second laminated polyester film of the present invention from the same viewpoint.
[0068] As the dicarboxylic acid component that is the raw material of the polyester resin, aromatic, aliphatic, and alicyclic dicarboxylic acids can be used. As the aromatic dicarboxylic acid, for example, terephthalic acid, isophthalic acid, orthophthalic acid, phthalic acid, 2,5-dimethylterephthalic acid, 1,4-naphthalenedicarboxylic acid, biphenyldicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 1,2-bisphenoxyethane-p-p'-dicarboxylic acid, phenylindanedicarboxylic acid, and 5-sulfoisophthalic acid can be used. As the aliphatic and alicyclic dicarboxylic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, dodecanedioic acid, dimer acid, 1,3-cyclopentanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, and the like, and their ester-forming derivatives can be used.
[0069] The diol components used as raw materials for polyester resins include ethylene glycol, diethylene glycol, polyethylene glycol, propylene glycol, polypropylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 2,4-dimethyl-2-ethylhexane-1,3-diol, neopentyl glycol, 2-ethyl-2-butyl-1,3-propanediol, 2-ethyl-2-isobutyl-1,3-propanediol, 3-methyl-1,5-pentanediol, 2,2,4-trimethyl-1,6-hexanediol, can be used. Examples of the compounds that can be used include 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 4,4'-thiodiphenol, bisphenol A, 4,4'-methylenediphenol, 4,4'-(2-norbornylidene)diphenol, 4,4'-dihydroxybiphenol, o-, m-, and p-dihydroxybenzene, 4,4'-isopropylidenephenol, 4,4'-isopropylidenebindiol, cyclopentane-1,2-diol, cyclohexane-1,2'-diol, cyclohexane-1,2-diol, cyclohexane-1,4-diol, and 1,4-butanediol dimethanesulfonate.
[0070] As the polyester resin, it is also possible to use modified polyester copolymers, for example, block copolymers and graft copolymers modified with acrylic, urethane, epoxy, or the like.
[0071] The polyester resin preferably has a functional group in the side chain, in order to form a dense coating film by crosslinking with the reactive compound c described below and to suppress the decrease in antistatic properties during transportation and processing. Examples of the functional group include hydroxyl, carboxyl, amide, glycidyl, isocyanate, and sulfo groups. The amount of functional group can be selected by using the acid value or hydroxyl value as a representative value. For example, if the acid value of the polyester resin is less than 5 KOH / mg, the applicability and adhesion of the water-based coating agent may decrease.
[0072] The acrylic resin is not particularly limited, but is preferably composed of alkyl methacrylate and / or alkyl acrylate. As the alkyl methacrylate and / or alkyl acrylate, it is preferable to use methacrylic acid, methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-hexyl methacrylate, lauryl methacrylate, 2-hydroxyethyl methacrylate, hydroxypropyl methacrylate, acrylic acid, methyl acrylate, ethyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-hexyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, hydroxypropyl acrylate, maleic acid, itaconic acid, acrylamide, N-methylol acrylamide, diacetone acrylamide, etc. These can be used alone or in combination of two or more. The acrylic resin is a dense resin with a small repeating polymer structure, and is therefore a material suitable for improving the abrasion resistance of the resin layer X, and is particularly preferred because it improves the durability of the antistatic properties.
[0073] The urethane resin is preferably a resin obtained by reacting a polyhydroxy compound with a polyisocyanate compound by a known urethane resin polymerization method such as emulsion polymerization, suspension polymerization, etc. Examples of the polyhydroxy compound include polyethylene glycol, polypropylene glycol, polyethylene propylene glycol, polytetramethylene glycol, hexamethylene glycol, tetramethylene glycol, 1,5-pentanediol, diethylene glycol, triethylene glycol, polycaprolactone, polyhexamethylene adipate, polyhexamethylene sebacate, polytetramethylene adipate, polytetramethylene sebacate, trimethylolpropane, trimethylolethane, pentaerythritol, polycarbonate diol, and glycerin. Examples of the polyisocyanate compound that can be used include hexamethylene diisocyanate, diphenylmethane diisocyanate, tolylene diisocyanate, isophorone diisocyanate, an adduct of tolylene diisocyanate and trimethylenepropane, an adduct of hexamethylene diisocyanate and trimethylolethane, etc. The above-mentioned urethane resin and its copolymer (for example, acrylic-urethane copolymer, urethane-modified polyester, etc.) are relatively flexible resins, and therefore can provide the effect of relieving stress when the resin layer X is worn.
[0074] Examples of the epoxy resin include sorbitol polyglycidyl ether crosslinking agents, polyglycerol polyglycidyl ether crosslinking agents, diglycerol polyglycidyl ether crosslinking agents, and polyethylene glycol diglycidyl ether crosslinking agents. Commercially available epoxy resins may be used, such as epoxy compounds "Denacol" (registered trademark) EX-611, EX-614, EX-614B, EX-512, EX-521, EX-421, EX-313, EX-810, EX-830, EX-850, etc., manufactured by Nagase Chemtec Corporation, diepoxy / polyepoxy compounds (SR-EG, SR-8EG, SR-GLG, etc.) manufactured by Sakamoto Pharmaceutical Co., Ltd., epoxy crosslinking agents "EPICLON" (registered trademark) EM-85-75W or CR-5L, manufactured by Dainippon Ink Mfg. Co., Ltd., and among these, those having water solubility are preferably used. The above epoxy resin has appropriate hydrophilicity and hydrophobicity, and is therefore considered to be a resin that is particularly effective in stabilizing the dispersion of the conductive component A. <Compound c> The resin layer X in the second laminated polyester film of the present invention must contain a reactive compound c in order to sufficiently advance the crosslinking reaction of the resin layer X and ensure the durability of the antistatic property, and it is preferable that the resin layer X in the first laminated polyester film of the present invention also contains the compound c from the above-mentioned viewpoint. As the compound c, an oxazoline compound, a carbodiimide compound, a melamine compound, or an isocyanate compound can be used alone or in combination, but from the viewpoint of designing the above-mentioned R3 / R1 value to be less than 3.0, it is preferable to use a melamine compound alone or in combination with other compounds. Note that even if the reactive compound c forms a different chemical structure derived from the compound between the resin component and the resin component through a crosslinking reaction or the like and the compound c does not exist in the resin layer X as a single substance, it can be interpreted that the resin layer X contains the compound c.
[0075] The oxazoline compound has an oxazoline group as a functional group in the compound, and is preferably an oxazoline group-containing copolymer obtained by copolymerizing at least one monomer containing an oxazoline group and at least one other monomer.
[0076] In the oxazoline compound, at least one other monomer used for the monomer containing an oxazoline group is a monomer copolymerizable with the monomer containing an oxazoline group, and examples thereof include acrylic acid esters or methacrylic acid esters such as methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, 2-ethylhexyl acrylate, and 2-ethylhexyl methacrylate, unsaturated carboxylic acids such as acrylic acid, methacrylic acid, itaconic acid, and maleic acid, and unsaturated nitriles such as acrylonitrile and methacrylonitrile. Examples of the monomers that can be used include unsaturated amides such as vinyl acetate, vinyl propionate, and vinyl ethers such as methyl vinyl ether and ethyl vinyl ether, olefins such as ethylene and propylene, halogen-containing α,β-unsaturated monomers such as vinyl chloride, vinylidene chloride, and vinyl fluoride, and α,β-unsaturated aromatic monomers such as styrene and α-methylstyrene. These monomers may be used alone or in combination as long as the scope of the present invention is satisfied.
[0077] Specific oxazoline compounds are not particularly limited, but addition-polymerizable oxazoline group-containing monomers are preferred, and examples thereof include 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 2-isopropenyl-4-methyl-2-oxazoline, and 2-isopropenyl-5-ethyl-2-oxazoline. These may be used alone or in combination as long as they satisfy the scope of the present invention.
[0078] The carbodiimide compound is a compound having at least one carbodiimide group or a cyanamide group having a tautomeric relationship therewith as a functional group in the molecule. Specific examples of such carbodiimide compounds include dicyclohexylmethanecarbodiimide, dicyclohexylcarbodiimide, tetramethylxylylenecarbodiimide, and urea-modified carbodiimide, and these may be used alone or in combination as long as they satisfy the scope of the present invention.
[0079] Examples of the melamine compound that can be used in the laminated polyester film of the present invention include a melamine compound having one or more triazine rings and one or more methylol groups in one molecule. By using such a melamine compound, a crosslinked structure between methylol groups can be formed in the resin layer X.
[0080] Examples of the melamine compound include melamine, methylolated melamine derivatives obtained by condensing melamine with formaldehyde, compounds obtained by reacting methylolated melamine with a lower alcohol to partially or completely etherify the melamine, and mixtures thereof. The melamine compound may be either a condensate of a monomer or a dimer or higher polymer, or a mixture thereof. Examples of the lower alcohol used for etherification include methyl alcohol, ethyl alcohol, isopropyl alcohol, n-butanol, and isobutanol. The functional group has an amino group, a methylol group, or an alkoxymethyl group such as a methoxymethyl group or a butoxymethyl group in one molecule, and examples of the methylated melamine compound include an amino group type methylated melamine compound, a methylol group type melamine compound, a methylol group type methylated melamine compound, and a fully alkylated methylated melamine compound. In particular, examples of methylol melamine compounds include monomethylol melamine, dimethylol melamine, trimethylol melamine, tetramethylol melamine, pentamethylol melamine, and hexamethylol melamine. These may be used alone or in combination as long as they satisfy the scope of the present invention.
[0081] <Compound d> In the second laminated polyester film of the present invention, compound d can be used to uniformly and finely disperse the conductive component A in the resin layer X. In the first laminated polyester film of the present invention, it is preferable that the resin layer X contains compound d from the same viewpoint. The type of compound d is not particularly limited, but it is preferable that the compound d is composed of any one of polystyrene sulfonate, polyvinylpyrrolidone-based polymer, water-soluble cellulose, or water-soluble cellulose derivative, or a combination thereof, from the viewpoint of increasing the dispersibility of the conductive component A, the compatibility with resin b and compound c, and improving the antistatic property and durability of the resin layer X. Representative examples of polystyrene sulfonate include sodium polystyrene sulfonate and calcium polystyrene sulfonate. Representative examples of polyvinylpyrrolidone-based polymers include polyvinylpyrrolidone.
[0082] Representative examples of water-soluble cellulose include hydroxycellulose and hydroxyalkylcellulose. Here, hydroxyalkylcellulose is cellulose in which the hydroxy group of the glucopyranose monomer constituting the cellulose skeleton is substituted with a hydroxyalkyl group (when the glucopyranose monomer has multiple hydroxy groups, it is sufficient that at least one of the hydroxy groups is substituted with a hydroxyalkyl group). Preferred examples include hydroxypropylmethylcellulose and hydroxyethylcellulose.
[0083] Representative examples of water-soluble cellulose derivatives include metal salts of carboxycellulose. Carboxycellulose is cellulose in which the hydroxyl group of the glucopyranose monomer constituting the cellulose skeleton is replaced with a carboxyl group (when the glucopyranose monomer has a plurality of hydroxyl groups, at least one of the hydroxyl groups is replaced with a carboxyl group). The term "carboxyl group" as used herein includes not only the carboxyl group in the narrow sense but also a carboxyalkyl group. Among the metal salts of carboxycellulose, metal salts of carboxyalkylcellulose are preferred because of their good water solubility, and more preferred are sodium carboxymethylcellulose and calcium carboxymethylcellulose, which are inexpensive and widely used industrially. Sodium carboxymethylcellulose is particularly preferred.
[0084] The above compound d may be used alone or in combination of two or more. In the present invention, polyvinylpyrrolidone, polyoxyalkylene derivatives, polystyrene sulfonic acid, cellulose derivatives, polycarboxylic acids, acrylic copolymers, and alkylbenzene sulfonates are preferred, and polyvinylpyrrolidone, polyoxyalkylene derivatives, polycarboxylic acids, and acrylic copolymers are more preferred because they provide better dispersibility of the carbon material. Compound d is also preferred if it has one or more branched chains and the molecular weight of the branched chain is 15 or more, since the molecular chain spreads in all directions and the dispersibility of the carbon material can be further improved. By using such compound d, when it is used in combination with resin b and compound c, or when the in-line coating method, which is a particularly preferred manufacturing method, is applied, cracking of the coating film due to stretching and disconnection of the conductive path are less likely to occur, and as a result, excellent antistatic properties and durability can be obtained. In addition, excellent transparency and slipperiness can be obtained by improving the dispersibility of the carbon material and by making it less likely to cause cracking of the coating film due to stretching when the in-line coating method, which is a particularly preferred manufacturing method, is applied.
[0085] <Method for preparing coating composition for forming resin layer X> The resin layer X is preferably formed by coating with a coating composition. When preparing the coating composition for this purpose, a solvent or a dispersion medium (hereinafter collectively referred to as solvent) may be included. That is, various components may be dissolved or dispersed in a solvent to form a coating composition, which may then be applied to a polyester substrate. When such a method is adopted, a laminated polyester film in which the resin layer X is laminated on the polyester film can be obtained by drying the solvent after application and heating.
[0086] In the laminated polyester film of the present invention, it is preferable to use an aqueous solvent E as the solvent. Here, the aqueous solvent E refers to a mixture of water or water and an organic solvent soluble in water, such as alcohols such as methanol, ethanol, isopropyl alcohol, butanol, ketones such as acetone, methyl ethyl ketone, glycols such as ethylene glycol, diethylene glycol, propylene glycol, etc., mixed in any ratio. By using the aqueous solvent E, it is possible to suppress the rapid evaporation of the solvent during the heating process, and not only can a more uniform resin layer X be formed, but it is also excellent in terms of environmental load.
[0087] A preferred coating composition for forming the resin layer X of the laminated polyester film of the present invention can be prepared by mixing and stirring the conductive component A, resin b, compound c, compound d, and aqueous solvent E, which are water-dispersed or water-soluble as necessary, in any order at a desired mass ratio. Next, various additives such as a lubricant, inorganic particles, organic particles, surfactants, antioxidants, and thermal initiators can be mixed and stirred in any order as needed to the extent that they do not deteriorate the properties of the resin layer X provided by the coating composition. The mixing and stirring method can be a method of shaking the container by hand, a method of stirring with a magnetic stirrer or stirring blade, a method of using ultrasonic irradiation, vibration dispersion, or the like.
[0088] Examples of the particles used include inorganic particles such as colloidal silica, titanium oxide, aluminum oxide, zirconium oxide, calcium carbonate, carbon black, and zeolite particles, and organic particles such as acrylic particles, silicone particles, polyimide particles, "Teflon" (registered trademark) particles, crosslinked polyester particles, crosslinked polystyrene particles, crosslinked polymer particles, and core-shell particles. These may be used alone or in combination of two or more kinds. Among them, inorganic particles are preferred, and colloidal silica is more preferred, from the viewpoint of hardness for obtaining the effect of suppressing blocking and heat resistance in a preferred manufacturing method of the laminated polyester film. As the colloidal silica, for example, the "Snowtex" (registered trademark) series manufactured by Nissan Chemical Industries, Ltd. and the "Cataloid (registered trademark)" series manufactured by JGC Catalysts and Chemicals Co., Ltd. can be suitably used.
[0089] The number average particle diameter of these particles is preferably in the range of 10 nm to 500 nm from the viewpoint of slipperiness. Here, the number average particle diameter is the value (number average) obtained by adding up the particle diameters of primary particles defined as particles generated by the growth of a single crystal nucleus in JIS H7008 (2002) and dividing by the number. The number average particle diameter of the particles is more preferably in the range of 20 nm to 300 nm, and further preferably in the range of 40 nm to 150 nm. The particles may be monodisperse particles or agglomerated particles in which a plurality of particles are agglomerated. In some cases, a plurality of types of particles having different number average particle diameters may be used in combination. The number average particle diameter of the particles can be measured by particle size distribution analysis using dynamic light scattering in the case of a coating composition, and by shape analysis using SEM-EDX in the case of a laminated polyester film.
[0090] A preferred coating composition for forming the resin layer X in the laminated polyester film of the present invention is specifically one that "contains a conductive component A, and is defined as resin b having a hydroxyl group, carboxyl group or sulfo group in a side chain, compound c is defined as a compound having at least one of a group of functional groups consisting of an amino group, a methylol group, a carbodiimide group and an oxazoline group, and compound d is defined as a compound having at least one branched chain, and further contains resin b, compound c and compound d." By satisfying the above combination, the "surface resistivity R1 of the resin layer X to be formed is 1.0×10 4 Ω / □ or more 1.0×10 10 Ω / □ or less, the ratio R2 / R1 value being less than 3.0, and the ratio R3 / R1 value being less than 3.0" are more easily achieved, thereby improving the antistatic properties and durability.
[0091] The content of the conductive component A is preferably 10 parts by mass or more and 80 parts by mass or less, and more preferably 20 parts by mass or more and 50 parts by mass or less, relative to 100 parts by mass of the resin b. By having the content of the conductive component A be 10 parts by mass or more and 80 parts by mass or less, relative to 100 parts by mass of the resin b, it becomes easier to keep the antistatic property within the range of the target of the present invention, and further, it becomes easier to obtain transparency, especially in display applications. The content of the compound c is preferably 5 parts by mass or more and 50 parts by mass or less, relative to 100 parts by mass of the resin b, and more preferably 10 parts by mass or more and 30 parts by mass or less. By having the content of the compound c be 5 parts by mass or more and 50 parts by mass or less, relative to 100 parts by mass of the resin b, it becomes possible to achieve both the dispersibility of the conductive component A and the stretchability and durability of the antistatic property in the in-line coating described later. The content of the compound d is preferably 0.1 parts by mass or less and 30 parts by mass or less, relative to 100 parts by mass of the conductive component A, and more preferably 0.5 parts by mass or more and 20 parts by mass or less. By making the content of compound d 0.1 parts by mass or less and 30 parts by mass or less per 100 parts by mass of conductive component A, it becomes easier to control the value of R3 / R1 of the formed resin layer X to less than 3.0 within the above-mentioned range, thereby improving the antistatic properties and durability.
[0092] <Method of manufacturing laminated polyester film> The method for forming the resin layer X of the present invention is not particularly limited, but a preferred method is to apply and heat the above-mentioned preferred coating composition to at least one surface of a polyester film to form the resin layer X. More specifically, a more preferred manufacturing method is a method for manufacturing a laminated polyester film, comprising step 1 of directly coating and laminating a polyester film with a coating composition containing a conductive component A, resin b, compound c, and compound d, and containing water as a main dispersion medium, where resin b is a resin having a hydroxyl group, carboxyl group, or sulfo group in a side chain, compound c is a compound having at least one of a group of functional groups consisting of an amino group, a methylol group, a carbodiimide group, and an oxazoline group, and compound d is a compound having one or more branched chains, step 2 of stretching the polyester film that has undergone step 1 in at least one axial direction, and step 3 of heating the polyester film that has undergone step 2 at 200°C or more and 260°C or less. In this forming method, the coating composition may contain, in addition to the above-mentioned preferred resins and compounds, various additives such as crosslinking catalysts, lubricants, inorganic particles, organic particles, surfactants, antioxidants, thermal initiators, etc. The main dispersion medium refers to a component contained in the dispersion medium in an amount of more than 50 mass % and not more than 100 mass %.
[0093] In step 1, in which a coating composition whose main dispersion medium is water is directly applied to a polyester film and laminated, either an in-line coating method or an off-coating method can be used as the coating method, but the in-line coating method is preferred. The in-line coating method is a method in which a coating composition is applied during the manufacturing process of a polyester substrate (polyester film). Specifically, it refers to a method in which coating is performed at any stage from melt extrusion of a polyester resin to biaxial stretching, followed by heat treatment and winding up. Usually, the coating is applied to any of the following films: an unstretched (unoriented) polyester film (hereinafter sometimes referred to as A film) in a substantially amorphous state obtained by melt extrusion and quenching, a uniaxially stretched (uniaxially oriented) polyester film (hereinafter sometimes referred to as B film) that has been stretched in the longitudinal direction, or a biaxially stretched (biaxially oriented) polyester film (hereinafter sometimes referred to as C film) that has been further stretched in the transverse direction and before heat treatment.
[0094] In the manufacturing method of the laminated polyester film of the present invention, it is preferable to adopt a method in which a coating composition is applied to either the A film or the B film of the polyester film before the crystal orientation is completed, the solvent is evaporated, and then the polyester film is stretched in a uniaxial or biaxial direction and heated to complete the crystal orientation of the polyester film, thereby providing the resin layer X. That is, it is a method in which a step 2 is provided in which the polyester film that has undergone the step 1 is stretched at least in a uniaxial direction. According to this method, the film formation of the polyester film (corresponding to the polyester substrate of the laminated polyester film of the present invention), the coating of the coating composition, the drying of the solvent, and the heating (i.e., the formation of the resin layer X) can be performed in a continuous step. In particular, when the coating is performed on the B film, the heat treatment step (thermal fixation) after the stretching in the width direction of the polyester film, and the drying and heating of the coating composition (i.e., the formation of the resin layer X by heat curing) can be performed in the same step. Therefore, not only is there an advantage in terms of manufacturing cost, but by completing the crystal orientation of the polyester substrate after drying, it is possible to perform a high-temperature heat treatment on the coating layer while reducing the deformation and thermal shrinkage of the substrate. As a result, crosslinking of the resin layer X formed by coating is promoted, and the antistatic properties are less likely to be lost even after long-distance transportation and multiple processing steps, especially processing steps including heating. Another advantage is that the thickness of the resin layer X can be easily made thinner and more uniform by stretching after coating.
[0095] In addition, there are preferable temperature conditions for the heat treatment (thermal curing) performed on the coating layer from the viewpoint of sufficiently proceeding the crosslinking reaction of the resin layer X and enhancing the durability of the antistatic layer. Specifically, the resin layer X is preferably formed by thermal curing at a heat treatment temperature of 170°C or more, more preferably 180°C or more, even more preferably 200°C or more, and particularly preferably 230°C or more. In addition, the upper limit of the heat treatment temperature is preferably 260°C in view of the heat resistance temperature of the polyester film. By setting the heat treatment temperature at 260°C or less, deformation of the polyester film is suppressed, and it is easy to obtain a more uniform laminated polyester film. That is, a preferable manufacturing method of the laminated polyester film of the present invention has a step 3 in which the polyester film that has been subjected to the step 2 is heated at 200°C or more and 260°C or less.
[0096] Among these, a method in which a coating composition is applied to a film (film B) uniaxially stretched in the longitudinal direction, the solvent is dried, and then the film is stretched in the width direction and heated is excellent. This is because, compared with a method in which a coating composition is applied to an unstretched film and then biaxially stretched, this method requires one less stretching step for the layer formed by the coating composition, making it difficult for defects or cracks to occur in the resin layer X due to stretching, and making it possible to form a resin layer X with excellent transparency and smoothness.
[0097] In addition, although different from the above-mentioned preferred method, an offline coating method can also be used. The offline coating method is a method in which the coating composition is applied to the film after the A film is uniaxially or biaxially stretched and heat-treated to complete the crystal orientation of the polyester film, or to the A film itself, in a process separate from the film-forming process. In the present invention, from the various advantages described above, it is preferable to use the in-line coating method, but even when the resin layer X is formed by the offline coating method, the processing temperature is preferably 170°C or higher, more preferably 180°C or higher, and even more preferably 200°C or higher. By setting the processing temperature to 170°C or higher, the crosslinking reaction can be promoted to sufficiently harden the thin resin layer X.
[0098] In particular, from the viewpoint of suppressing the penetration of the water-based coating material by sufficiently advancing the crosslinking reaction of the resin layer X, even if the same formulation is used, it may be difficult to lower R3 / R1 unless the processing temperature is 170°C or higher. The upper limit of the processing temperature is preferably 260°C in view of the heat resistance temperature of the polyester film. By keeping the processing temperature at 260°C or lower, deformation of the polyester film is suppressed, making it easier to obtain a uniform laminated polyester film.
[0099] Here, the method of applying the coating composition to the polyester film can be any method selected from known coating methods, such as bar coating, reverse coating, gravure coating, die coating, blade coating, etc., for both in-line coating and offline coating.
[0100] Therefore, a preferred method for forming the resin layer X in the present invention is a method in which a coating composition using an aqueous solvent is applied to a polyester substrate by in-line coating, followed by drying and heat treatment. More preferably, the coating composition is in-line coated on the B film after uniaxial stretching. In the method for producing the laminated polyester film of the present invention, the drying is preferably carried out at a temperature range of 80 to 130°C in order to complete removal of the solvent from the coating composition. The heat treatment is preferably carried out at a temperature range of 170 to 260°C, preferably 200 to 260°C, in order to complete the crystal orientation of the polyester film and the thermal curing of the coating composition to complete the formation of the resin layer X.
[0101] Next, the method for producing the laminated polyester film of the present invention will be explained in more detail using an example in which a polyethylene terephthalate (hereinafter, PET) film is used as the polyester base material; however, the laminated polyester film of the present invention and its production method are not limited thereto.
[0102] First, PET pellets are thoroughly vacuum-dried, then fed into an extruder, melt-extruded into a sheet at 260-280°C, and cooled and solidified to produce an unstretched (unoriented) PET film (A film). (In this case, the sheet-like material melt-extruded into a sheet is preferably cooled and solidified using a cast drum at a temperature of 10-40°C.) This unstretched PET film is stretched 2.5-5.0 times in the longitudinal direction using a roll heated to 80-120°C to obtain a uniaxially oriented PET film (B film). Furthermore, the aforementioned coating composition (a coating composition containing conductive component A, the resin b, the compound c, and the compound d, and in which the main dispersion medium is water) prepared to a predetermined concentration is applied to one side of this B film.
[0103] At this time, the surface of the uniaxially oriented PET film to be coated may be subjected to a surface treatment such as a corona discharge treatment before the coating composition is applied. By performing a surface treatment such as a corona discharge treatment, the wettability of the coating composition to the uniaxially oriented PET film is improved, so that the coating composition is prevented from being repelled, and a resin layer X having a more uniform coating thickness can be formed. After the coating composition is applied, the ends of the uniaxially oriented PET film are held with clips and the solvent of the coating composition is dried in a heat treatment zone (preheating zone) at 80 to 130 ° C. In particular, when the uniaxially oriented PET film coated with the coating composition is sent to the heat treatment zone, it is preferable to carry out the process by holding the uncoated parts at both ends of the width direction of the uniaxially oriented PET film with clips and leading it to a tenter. After drying, the film is stretched 1.1 to 5.0 times in the width direction, and then led to a heat treatment zone (thermal fixation zone) at 170 to 260 ° C., preferably 200 to 260 ° C., where it is heat treated for 1 to 30 seconds to complete the crystal orientation.
[0104] In this heat treatment step (thermal fixation step), a 3 to 15% relaxation treatment may be performed in the width direction or the length direction as necessary. Thereafter, the laminated polyester film is cooled to room temperature, and the laminated polyester film is cut parallel to the length direction with a known razor blade or the like to remove the uncoated parts at both ends in the width direction that were held by the clips, and then the film can be wound into a roll. The laminated polyester film thus obtained is a laminated polyester film that has excellent applicability, adhesion, and transparency of water-based coating materials. The uncoated parts of the film at both ends in the width direction cut and removed by the slitter can be used as the above-mentioned recycled raw material from the viewpoint of environmental consideration.
[0105] In the laminated polyester film of the present invention, an intermediate layer may be provided between the resin layer X and the polyester base material, but when an intermediate layer is provided, the film may be scratched when the film having the intermediate layer laminated thereon is wound up or in the subsequent process up to the provision of the resin layer X of the present invention. Therefore, in the present invention, it is preferable that the resin layer X and the polyester base material are directly laminated.
[0106] The polyester film constituting the laminated polyester film of the present invention is not limited in its layer structure, and examples thereof include a single-layer structure consisting of only Layer A, a laminate structure of Layer A / Layer B, i.e., a two-type two-layer laminate structure, a laminate structure of Layer A / Layer B / Layer A, i.e., a two-type three-layer laminate structure, and a laminate structure of Layer A / Layer B / Layer C, i.e., a three-type three-layer laminate structure.
[0107] The lamination method of the polyester film, which is the base material constituting the laminated polyester film of the present invention, is not limited, and examples thereof include lamination methods by coextrusion, lamination methods by lamination, and combinations thereof. From the viewpoint of transparency and manufacturing stability, it is preferable to adopt the coextrusion method. When forming a laminate, different resin structures may be used to impart different functions to each layer. For example, when forming a laminate structure of A layer / B layer / A layer, that is, a two-kind three-layer structure, the B layer may be made of homopolyethylene terephthalate from the viewpoint of transparency, and particles may be added to the A layer to impart easy slippage.
[0108] <Resin layer Y> The laminated polyester film of the present invention can be a laminate in which a resin layer Y is laminated directly or via an intermediate layer on the surface opposite to the resin layer X. The resin layer Y may be any layer as long as it does not impair the function of the present invention, and can be, for example, any of an adhesive layer, a heat seal layer, and a release layer. The method for laminating the resin layer Y may be either lamination by coating or lamination by lamination, but lamination by coating such as bar coating, reverse coating, gravure coating, die coating, and blade coating is preferred. In order to control the adhesion with the resin layer Y, it is also preferred to laminate via an adhesive layer or to laminate after performing a known adhesion improving treatment such as corona treatment or plasma discharge treatment.
[0109] The laminate of the present invention has an antistatic effect, which makes it possible to avoid deterioration in quality and yield, such as damage to components and inspection defects caused by discharge, and also has good dust resistance and scratch resistance, and therefore can be suitably used as an adhesive film in the manufacturing process of display components such as OLEDs, a film in the manufacturing process of packaging materials such as cover tapes, and a release film in the manufacturing process of electronic components such as ceramic green sheets. EXAMPLES
[0110] Next, the present invention will be described in more detail with reference to examples, but is not necessarily limited thereto. The methods for measuring the various characteristics and the methods for evaluating the various effects in the present invention are as follows.
[0111] [Methods of measuring characteristics and evaluating effects] (1) Thickness of Resin Layer X The thickness of the resin layer X on the polyester substrate was measured by observing the cross section using a transmission electron microscope (TEM). The thickness of the resin layer X was read from an image taken with a TEM at a magnification of 200,000 times. The thickness of the resin layer X was measured at a total of 20 points, and the average value was taken as the thickness of the resin layer X.
[0112] (2)Surface resistivity The surface resistivity was measured by preparing the laminated film to be measured, leaving it at 60% relative humidity and 23°C for 24 hours, and then measuring it in that atmosphere using a digital ultra-high resistance / micro ammeter R8340A and a resistivity chamber 12702A (manufactured by Advantest Corporation, main electrode: Φ50mm, counter electrode: Φ103mm) after applying a voltage of 100V for 10 seconds. The unit of surface resistivity is Ω / □. The resin layer X side of the laminated polyester film was evaluated, and the average value of a total of 10 measurements was taken as the surface resistivity of the sample.
[0113] (3) Measurement of total light transmittance and haze Five square laminated polyester film samples, each 5 cm on a side, were prepared. The samples were then left to stand for 40 hours at a relative humidity of 60% and 23°C. The total light transmittance and haze of each sample were measured using a turbidity meter "NDH5000" manufactured by Nippon Denshoku Industries Co., Ltd., in accordance with the method specified in JIS "Determining Haze of Transparent Materials" (K7136 2000 edition). The total light transmittance and haze values of each of the five samples were averaged to obtain the total light transmittance and haze values of the laminated polyester film.
[0114] (4) Film handling Two laminated polyester film samples cut to the size of an A4 sheet were prepared. The surface of one laminated polyester film having the resin layer X was brought into contact with the surface of the other laminated polyester film opposite to the surface having the resin layer X so that the four sides of the sheets overlapped, and the two were pressed together with a rubber roller weighing 2 kg so that no air remained. The two laminated polyester films were then rubbed against each other by moving them back and forth in a staggered manner for about 10 cm in the longitudinal direction. The sheets were again placed together so that the four sides of the sheets coincided, and then pressed together with a rubber roller weighing 2 kg so that no air remained. Next, with the two laminated polyester films overlapping, a square with a side length of 10 cm was cut from the center of the A4 sheet. After leaving the obtained square-shaped film to stand, the upper laminated polyester film was lifted up from the corner position by pinching it with ceramic tweezers. The handling properties of the film were evaluated according to the behavior of the laminated polyester film when handled in the above procedure, using the following four stages. A: The films were able to be lifted without sticking together. B: The films stuck together but fell off under their own weight. C: The films stuck together but could be easily peeled off. D: The films were strongly attached to each other and required force to peel them off, or peeling was impossible.
[0115] (5) Heat treatment characteristics For the heat treatment evaluation assuming long-distance transportation of the laminated polyester film or use in multiple processing steps, two laminated polyester film samples cut to A4 sheet size were stacked in the same manner as in (4), and then pressed 10 times under conditions of a temperature of 180°C, a pressure of 0.3 mPa, and a speed of 0.5 m / min using a roll laminator manufactured by Tester Sangyo Co., Ltd. Next, in the same manner as in (4), a square with a side length of 10 cm was cut from the center of the A4 sheet, and the handleability of the film was evaluated. A: The films were able to be lifted without sticking together. B: The films stuck together but fell off under their own weight. C: The films stuck together but could be easily peeled off. D: The films were strongly attached to each other and required force to peel them off, or peeling was impossible.
[0116] (6) Measurement of static friction coefficient Ten pieces of laminated polyester film with a size of 7.5cm x 10cm were cut out and left to stand at a relative humidity of 60% and 23°C for 12 hours. Then, under that atmosphere, two samples were stacked so that the resin layer X-sides faced each other, and the end of the upper sample was attached to a load cell with double-sided adhesive tape 801 (0.1mm x 10mm x 20m) made by Nichiban Co., Ltd., and the end of the lower sample opposite the load cell side was attached to a base with double-sided adhesive tape No. 532 (0.08mm x 20mm x 50m) made by Nitto Denko Co., Ltd., and a load of 200g was applied to the stacked samples and measured at a speed of 120mm / min. The measurement was performed five times with different samples, and the static friction coefficients obtained at the five points were averaged to obtain the value of the static friction coefficient of the laminated polyester film.
[0117] [Resins, etc. used in the manufacture of laminated polyester film] [Conductive component A] Conductive component A1: 1.0 mg of straight double-walled CNT (manufactured by Science Laboratories, Inc., diameter 5 nm, aspect ratio 3000) as CNT, 3.0 mg of CNT dispersant sodium carboxymethylcellulose (manufactured by Sigma-Aldrich Japan Co., Ltd.) (hereinafter referred to as CMC-Na) and 666 mg of water were placed in a sample tube to prepare a CNT water dispersion, which was then irradiated with ultrasonic waves for 30 minutes using an ultrasonic crusher (Tokyo Rikakiki Co., Ltd. VCX-502, output 250 W, direct irradiation) to obtain a CNT water dispersion (D-1) (CNT concentration 0.15 wt%, CNT dispersant 0.45 wt%, CNT dispersant / CNT = 3.0) consisting of uniform CNT and CNT dispersant. This was designated as conductive component A1.
[0118] Conductive component A2: 49 parts by mass of a 1% by mass iron (III) sulfate aqueous solution, 8.8 parts by mass of 3,4-ethylenedioxythiophene as a thiophene compound, and 117 parts by mass of a 10.9% by mass peroxodisulfuric acid aqueous solution were added to 1887 parts by mass of an aqueous solution containing 20.8 parts by mass of polystyrene sulfonic acid, an acidic polymer compound. The mixture was stirred at 18°C for 23 hours, and 154 parts by mass of a cation exchange resin ("Lewatit" (registered trademark) Monoplus S100H; manufactured by Lanxess Co., Ltd.) and 232 parts by mass of an anion exchange resin ("Lewatit" (registered trademark) Monoplus M800; manufactured by Lanxess Co., Ltd.) were added to the mixture, and the mixture was stirred for 2 hours. The ion exchange resin was then filtered off to obtain an antistatic agent (D-2) (solid concentration 1.3% by weight) consisting of a mixture of poly(3,4-ethylenedioxythiophene) and polystyrene sulfonic acid. This was designated as conductive component A2.
[0119] [Resin b] Resin b1: Under a nitrogen gas atmosphere and at room temperature (25°C), 100 parts by mass of water, 1 part by mass of sodium lauryl sulfate, and 0.5 parts by mass of ammonium persulfate were charged into a container 1, which was then heated to 70°C to dissolve sodium lauryl sulfate, and a solution 1 at 70°C was obtained. Under room temperature (25°C), 30 parts by mass of water and 2 parts by mass of sodium lauryl sulfate were added to a container 2 to dissolve sodium lauryl sulfate, and then 13.3 parts by mass of polyethylene oxide monomethacrylate (10 repeating units of ethylene oxide) was added as an acrylic monomer component having a polyalkylene oxide, and 29.7 parts by mass of ethyl acrylate, 50.0 parts by mass of methyl methacrylate, and 5.0 parts by mass of N-methylol acrylamide were added as other monomer components, and the mixture was stirred to obtain a solution 2. Under a nitrogen gas atmosphere, the solution 1 was transferred to a reactor, and while maintaining the temperature of the solution in the reactor at 70°C, the solution 2 was continuously dripped into the solution 1 over a period of 3 hours. After the dropwise addition was completed, the mixture was stirred at 85° C. for an additional 2 hours, and then cooled to 25° C. to terminate the reaction, thereby obtaining an acrylic resin emulsion, designated as resin b1.
[0120] Resin b2: 45.0 parts by mass of CR-5L (solid content concentration 100% by weight) manufactured by DIC Corporation as an epoxy crosslinking agent and 5.0 parts by mass of a polyglycerol polyglycidyl ether-based epoxy crosslinking agent ("Denacol" (registered trademark) EX-512 (molecular weight about 630, epoxy equivalent 168, water solubility 100%) manufactured by Nagase Chemtec Corporation) were dissolved in 50.0 parts by mass of water to obtain an aqueous dispersion of epoxy compound (c). This was designated as resin b2.
[0121] Resin b3: 200.0 parts by mass of the copolymerization components shown below and 0.1 parts by mass of potassium titanium oxalate as a catalyst were added to a reactor, and the temperature was raised to 200°C while stirring and mixing in a nitrogen atmosphere at normal pressure. Next, the reaction temperature was gradually raised to 250°C over 4 hours to terminate the transesterification reaction. 15 parts by mass of the polyester resin thus obtained and 85 parts by mass of water were added to a dissolution tank and dispersed at a temperature of 80 to 95°C over 2 hours with stirring to obtain a 15% by mass aqueous dispersion of the polyester resin. This was designated as resin b3.
[0122] <Copolymerization component> (Dicarboxylic acid component) Dimethyl 2,6-naphthalenedicarboxylate: 88 mol% Sodium dimethyl 5-sulfoisophthalate: 12 mol% (Diol component) Compound with 2 moles of ethylene oxide added to 1 mole of bisphenol S: 86 mole% 1,3-propanediol: 14 mol% [Compound c] Compound c1: Melamine resin water sol ("WATERSOL" (registered trademark) S-695, manufactured by DIC Corporation) was used. Compound c2: An oxazoline-containing polymer aqueous dispersion ("Epocross" (registered trademark) WS-500, manufactured by Nippon Shokubai Co., Ltd.) was used. Compound c3: A carbodiimide water-based crosslinking agent ("Carbodilite" (registered trademark) V-04, manufactured by Nisshinbo Chemical Inc.) was used. Compound 4: Branched isocyanate compound (Elastron (registered trademark) E-37, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) [Compound d] Compound d1: Polyvinylpyrrolidone ("Polyvinylpyrrolidone K30" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used. Compound d2: A dodecylbenzenesulfonic acid catalyst ("NACURE" (registered trademark) 5528 manufactured by Kusumoto Chemicals Co., Ltd.) was used.
[0123] [Surfactants] Surfactant 1: An acetylene diol-based surfactant (Olfine (registered trademark) EXP.4200 manufactured by Nissin Chemical Industry Co., Ltd.) was used.
[0124] [particle] Inorganic particles 1: Silica particles having a number average particle size of 100 nm ("Snowtex" (registered trademark) MP-1040, manufactured by Nissan Chemical Industries, Ltd.).
[0125] Inorganic particles 2: Silica particles having a number average particle diameter of 22 nm ("Snowtex" (registered trademark) ST-50-T, manufactured by Nissan Chemical Industries, Ltd.).
[0126] Inorganic particles 3: Silica particles having a number average particle size of 500 nm ("Seahoster" (registered trademark) KE-W50, manufactured by Nippon Shokubai Co., Ltd.).
[0127] The number average molecular weight can be determined from the analysis of particle images observed by a cross-sectional transmission electron microscope (TEM) in the case of a film, and from number-based analysis by a dynamic light scattering (DLS) method in the case of a coating composition.
[0128] Example 1 <Paint composition> First, conductive component A1: resin b1: compound c1: compound d1: inorganic particle 1 were mixed in a ratio of 50:100:30:5:0.5 (mass ratio). After adjusting the concentration with water as a solvent, 0.1 parts by mass of surfactant 1 was added to a total of 100 parts by mass of water to adjust the coating property. Here, the method of adjusting the concentration with water will be described in detail. Specifically, the concentration was determined according to the target thickness of resin layer X by the following method. The thickness of resin layer X is proportional to the concentration of the coating composition and the coating thickness, and inversely proportional to the widthwise stretching ratio and the specific gravity of resin layer X. Of these, the coating thickness is uniquely determined from the number used for the bar coat, and the stretching ratio is uniquely determined from the film formation conditions. Therefore, a calibration curve was created by measuring the thickness of resin layer X by the above-mentioned method, and the concentration of the coating composition that matches the target thickness of resin layer X was determined. The concentration of the obtained coating composition was approximately 1.0% by mass to 3.0% by mass. In this way, the coating composition was obtained.
[0129] <Laminated polyester film> PET pellets (intrinsic viscosity 0.64 dl / g) containing two types of particles (4% by mass of silica particles with a primary particle size of 0.3 μm and 2% by mass of calcium carbonate particles with a primary particle size of 0.8 μm) were thoroughly vacuum dried, fed into an extruder and melted at 280°C, extruded into a sheet from a T-shaped nozzle, and wrapped around a mirror-finished casting drum with a surface temperature of 25°C by an electrostatic casting method, where it was cooled and solidified. The composition and particle size of the particles contained in the PET pellets were measured by a combination of shape analysis by TEM and elemental analysis by energy dispersive X-ray spectroscopy (EDX) on thin-film sections prepared using a cryomicrotome. On the other hand, the intrinsic viscosity was measured by an extrapolation method according to JIS K 7367:2002, in which PET pellets were dissolved in a solvent in which they could be dissolved (e.g., hexafluoroisopropanol), and the viscosity was measured at multiple concentrations. The viscosity at 100% (i.e., the intrinsic viscosity) was then calculated from the approximation curve.
[0130] The unstretched film (A film) thus obtained was heated to 90°C and stretched 3.1 times in the longitudinal direction to obtain a uniaxially stretched film (B film). The uniaxially stretched film was then subjected to a corona discharge treatment in air, and the above coating composition was applied using a bar coater (wire bar #4). The uniaxially stretched film to which the coating composition was applied was then held at both ends in the width direction with clips and introduced into a preheating zone. The atmospheric temperature in the preheating zone was set to 90 to 100°C, and the solvent in the coating composition was dried. The film was then continuously stretched 3.6 times in the width direction in a 100°C stretching zone, and heat-treated for 20 seconds in a 240°C heat treatment zone to form a resin layer X. The film was then subjected to a 5% relaxation treatment in the width direction at the same temperature to obtain a laminated polyester film in which the crystal orientation of the polyester film was completed. In the obtained laminated polyester film, the thickness of the PET film (polyester substrate) was 50 μm, and the thickness (film thickness) of the resin layer X was 15 nm. The evaluation results are shown in Tables 2 and 3.
[0131] (Examples 2, 4-7, 9-19, Comparative Examples 1-4) A laminated polyester film was obtained in the same manner as in Example 1, except that the coating composition was as shown in Table 1. The evaluation results are shown in Tables 2 and 3.
[0132] Example 3 A laminated polyester film was obtained by the following method using the coating composition of Example 2. A PET film "Lumirror" (registered trademark) T60 (substrate thickness 50 μm) manufactured by Toray Industries, Inc. was used as the substrate. The coating composition was applied onto the substrate using a wire bar, and then dried and cured by heat treatment at 180°C for 2 minutes in a hot air oven. In the obtained laminated polyester film, the PET film had a thickness of 50 μm, and the resin layer X had a thickness (film thickness) of 15 nm. The evaluation results are shown in Tables 2 and 3.
[0133] Example 8 A laminated polyester film was obtained in the same manner as in Example 1, except that the coating composition of Example 1 was used and the concentration was adjusted so that the thickness (film thickness) of the resin layer X was 40 nm. The evaluation results are shown in Tables 2 and 3. The thickness of the resin layer X was adjusted by changing the width of the groove of the wire bar.
[0134] [Table 1]
[0135] [Table 2]
[0136] [Table 3] [Industrial Applicability]
[0137] The present invention relates to a laminated polyester film whose antistatic properties are not easily impaired even when it is transported over long distances or undergoes a number of treatment steps, particularly a treatment step involving heating. The present invention can be used in the production processes of display components such as antireflection films, diffusion sheets, prism sheets, and transparent touch panels used in flat displays and the like, magnetic recording materials, packaging materials such as cover tapes, electronic components such as ceramic green sheets and various circuit materials, and battery components such as electrode components, and can be particularly suitably used in products that include post-processing steps including dry heat treatment.
Claims
1. A laminated polyester film having a resin layer X on at least one surface of a polyester film, the resin layer X containing a conductive component A, the resin layer X having a surface resistivity of R1, the resin layer X having a surface resistivity of R2 after a voltage of 500 V is applied for 120 seconds, and the resin layer X having a surface resistivity of R3 after heating at 100° C. for 24 hours, the laminated polyester film having all of the following characteristics 1 to 3: Feature 1: The R1 is 1.0×10 4 Ω / □ or more 1.0×10 10 Ω / □ or less. Feature 2: The value of R2 / R1 is less than 3.
0. Feature 3: The value of R3 / R1 is less than 3.
0.
2. A laminated polyester film having a resin layer X on at least one surface of a polyester film, the resin layer X containing a conductive component A, a resin having a hydroxyl group, a carboxyl group or a sulfo group in a side chain being referred to as resin b, a compound having at least one of a group of functional groups consisting of an amino group, a methylol group, a carbodiimide group and an oxazoline group being referred to as compound c, and a compound having at least one branched chain being referred to as compound d, the resin layer X further containing the resin b, the compound c and the compound d.
3. 2. The laminated polyester film according to claim 1, wherein the R2 / R1 is less than 1.
0.
4. 4. The laminated polyester film according to claim 1, wherein the conductive component A contains single-walled or double-walled carbon nanotubes having a diameter of 1 nm or more and 50 nm or less.
5. 4. The laminated polyester film according to claim 1, wherein the resin layer X comprises a resin b having a hydroxyl group, a carboxyl group or a sulfo group in a side chain, and a compound c having at least one functional group selected from the group consisting of an amino group, a methylol group, a carbodiimide group and an oxazoline group.
6. The laminated polyester film according to claim 1 or 3, wherein the resin layer X contains a compound d, the compound having at least one branched chain being defined as the compound d.
7. The laminated polyester film according to any one of claims 1 to 3, which can be used as a base substrate for coating in a manufacturing process of at least one of a group of members consisting of display members, electronic members, and battery members.
8. A laminate having a resin layer Y on the opposite side of the laminated polyester film according to any one of claims 1 to 3 to the resin layer X, directly or through an intermediate layer, wherein the resin layer Y is any one of an adhesive layer, a heat seal layer, and a release layer.
9. A method for producing the laminated polyester film according to any one of claims 1 to 3, comprising the steps of: step 1 of directly coating a polyester film with a coating composition, the coating composition containing a conductive component A, resin b, compound c, and compound d, and containing water as a main dispersion medium, where b is a resin having a hydroxyl group, a carboxyl group, or a sulfo group in a side chain; c is a compound having at least one of a group of functional groups consisting of an amino group, a methylol group, a carbodiimide group, and an oxazoline group; and d is a compound having at least one branched chain; step 2 of stretching the polyester film that has been subjected to step 1 in at least one uniaxial direction; and step 3 of heating the polyester film that has been subjected to step 2 at a temperature of 200°C to 260°C.
Citation Information
Patent Citations
Biaxially oriented polyester film
JP1986204240A
Laminated film and manufacturing process thereof
JP2004058648A
Transparent conductive film, transparent conductive laminate, three-dimensional display and resin composition
JP2018135492A
Laminated polyester film
JP2021171949A
Conductive film and method for producing the same
WO2009041170A1