Laminated glass for displaying projected image, windshield glass, and image display system

The laminated glass system with a luminescent and reflective layer addresses the challenge of displaying complex content in vehicle displays by enabling both virtual and real image projection, enhancing compatibility and visibility for drivers and passengers.

WO2024203686A1PCT designated stage expired Publication Date: 2024-10-03FUJIFILM CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010935
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-03-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing image display systems for vehicles, particularly in head-up displays, struggle to effectively display both virtual and real images, leading to compatibility issues as the content becomes more complex.

Method used

A laminated glass system incorporating a luminescent layer with binder resin and luminescent materials, along with a reflective layer, is used to create an image display system capable of showing both virtual and real images, where the luminescent layer and reflective layer are strategically positioned between glass plates, enhancing display capabilities.

Benefits of technology

The system allows for the selective display of virtual and real images, improving compatibility and visibility by enabling the driver to see essential information like direction while passengers can view additional details like time, with high contrast and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010935_03102024_PF_FP_ABST
    Figure JP2024010935_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides an image display system capable of displaying both a virtual image and a real image, and a laminated glass used therefor. The laminated glass according to the present invention comprises: a light-emitting layer containing a binder resin and at least one light-emitting material selected from the group consisting of light-emitting particles, a light-emitting pigment, and a light-emitting dye; and a reflective layer.
Need to check novelty before this filing date? Find Prior Art

Description

Laminated glass for projection display, windshield glass and image display system

[0001] The present invention relates to a laminated glass having a light-emitting layer and a reflective layer, a windshield glass, and an image display system.

[0002] By incorporating a film into laminated glass used in automobile windshields, etc., the film (laminated glass) can be used as a projection image display component in a head-up display system. For example, Patent Document 1 discloses the use of a film including a retardation layer and multiple cholesteric liquid crystal layers as a projection image display component in a head-up display system installed in an automobile. Typically, laminated glass for automobiles has an interlayer between two glass sheets. Patent Document 1 describes a system in which a laminated glass windshield glass displays a virtual image by providing a film on the interlayer. Patent Document 2 also describes a system in which a laminated glass interlayer having a luminescent layer containing a binder resin and at least one luminescent material selected from the group consisting of luminescent particles, luminescent pigments, and luminescent dyes is used as a projection image display component to display a real image. Meanwhile, in recent years, the content displayed on head-up displays has become more complex and diverse, making existing image display systems insufficient to accommodate this. To address the above-mentioned issues, the present inventors invented an image display system capable of displaying both virtual and real images.

[0003] International Publication No. 2016 / 052367 Japanese Patent Application Laid-Open No. 2014-24312

[0004] The present invention provides an image display system capable of displaying both virtual and real images, and laminated glass for use therein.

[0005] The present invention provides the following:

[0006] [1] A laminated glass comprising a pair of glass plates, a luminescent layer containing a binder resin and a luminescent material comprising at least one selected from the group consisting of luminescent particles, luminescent pigments, and luminescent dyes, and a reflective layer. [2] The laminated glass according to [1], further comprising an adhesive layer. [3] The laminated glass according to [1] or [2], further comprising a transparent resin substrate. [4] The laminated glass according to [1], further comprising an adhesive layer and a transparent resin substrate, wherein the adhesive layer, transparent resin substrate, reflective layer, and luminescent layer are sandwiched in this order between the pair of glass plates. [5] The laminated glass according to [1], wherein the luminescent layer is sandwiched between the pair of glass plates, and the adhesive layer, reflective layer, and transparent resin substrate are placed in this order on the glass plates opposite the luminescent layer. [6] The laminated glass according to [5], further comprising a hard coat layer on the transparent resin substrate opposite the reflective layer. [7] The laminated glass according to any of [1] to [6], wherein the reflective layer comprises a metal layer and a dielectric layer. [8] A windshield glass having the laminated glass according to any one of [1] to [7]. [9] An image display system having the laminated glass according to any one of [1] to [7], an imager that irradiates the laminated glass with projection image light, and an irradiation device that irradiates the laminated glass with light rays.

[0007] The present invention provides an image display system capable of displaying both virtual and real images, and laminated glass for use therein. More specifically, the present invention provides laminated glass characterized by having a reflective layer and a light-emitting layer containing a binder resin and at least one light-emitting material selected from the group consisting of light-emitting particles, light-emitting pigments, and light-emitting dyes. The present invention can also provide a windshield glass and an image display system.

[0008] Fig. 1 is a schematic diagram showing an example of laminated glass of the present invention. Fig. 2 is a schematic diagram showing an example of laminated glass of the present invention. Fig. 3 is a schematic diagram showing an example of laminated glass of the present invention. Fig. 4 is a schematic diagram showing an example of laminated glass of the present invention. Fig. 5 is a schematic diagram showing an example of laminated glass of the present invention. Fig. 6 is a schematic diagram showing an example of laminated glass of the present invention.

[0009] Below, a laminated glass, a windshield, a laminated glass for projected image display, and an image display system each characterized by having a light-emitting layer and a reflective layer will be described in detail based on preferred embodiments shown in the accompanying drawings. Note that the drawings described below are merely illustrative for explaining the present invention, and the present invention is not limited to the drawings shown below. Note that in the following, the range of values ​​indicated by "to" includes the values ​​written on both sides. For example, ε 1 is the number α 1 ~Number β 1 That is, ε 1 The range of α 1 and the number β 1 The range includes α 1 ≦ε 1 ≦β 1 Unless otherwise specified, angles such as "angles expressed by specific numerical values," "parallel," "perpendicular," and "orthogonal" include the generally accepted error range in the relevant technical field. Furthermore, "the same" includes the generally accepted error range in the relevant technical field, and "over the entire surface" also includes the generally accepted error range in the relevant technical field.

[0010] When referring to circularly polarized light, the term "selective" means that the amount of either the right-handed circularly polarized component or the left-handed circularly polarized component of light is greater than the other circularly polarized component. Specifically, when referring to "selectively," the degree of circular polarization of light is preferably 0.3 or more, more preferably 0.6 or more, and even more preferably 0.8 or more. It is even more preferably substantially 1.0. Here, the degree of circular polarization is defined as the intensity of the right-handed circularly polarized component of light, expressed as I R , the intensity of the left circularly polarized component is I L When this is the case, |I R -I L | / (I R +I L ) is the value expressed as

[0011] The "sense" of circularly polarized light refers to whether it is right-handed or left-handed. The sense of circularly polarized light is defined as follows: when viewed as if the light is traveling toward you, if the tip of the electric field vector rotates clockwise as time increases, it is right-handed, and if it rotates counterclockwise, it is left-handed.

[0012] The term "sense" is sometimes used to refer to the twist direction of the helix of cholesteric liquid crystals. When the twist direction (sense) of the helix of a cholesteric liquid crystal is right-handed, it reflects right-handed circularly polarized light and transmits left-handed circularly polarized light, and when the sense is left-handed, it reflects left-handed circularly polarized light and transmits right-handed circularly polarized light.

[0013] Unless otherwise specified, the term "light" refers to visible light and natural light (unpolarized). Visible light is electromagnetic light with wavelengths visible to the human eye, and typically refers to light in the wavelength range of 380 to 780 nm. Invisible light is light in the wavelength range of less than 380 nm or greater than 780 nm. Furthermore, within visible light, light in the wavelength range of 420 to 490 nm is blue (B) light, light in the wavelength range of 495 to 570 nm is green (G) light, and light in the wavelength range of 620 to 750 nm is red (R) light, although this is not limited thereto.

[0014] "Visible light transmittance" refers to the visible light transmittance for an A-light source as defined in JIS (Japanese Industrial Standards) R3212:2015 (Testing Methods for Automotive Safety Glass). That is, the transmittance is determined by measuring the transmittance at each wavelength in the range of 380 to 780 nm using a spectrophotometer with an A-light source, and multiplying the transmittance at each wavelength by a weighting coefficient obtained from the wavelength distribution and wavelength interval of the CIE (Commission Internationale de l'Eclairage) photopic standard relative luminosity factor, and calculating a weighted average. When simply referring to "reflected light" or "transmitted light," this term is used to include scattered light and diffracted light.

[0015] The polarization state of each wavelength of light can be measured using a spectroradiometer or a spectrometer equipped with a circular polarizer. In this case, the intensity of light measured through a right circular polarizer is I. R , the light intensity measured through a left circular polarizer is I L It can also be measured by attaching a circular polarizer to an illuminance meter or optical spectrometer. The ratio can be determined by attaching a right-handed circularly polarized light transmitting plate and measuring the amount of right-handed circularly polarized light, and by attaching a left-handed circularly polarized light transmitting plate and measuring the amount of left-handed circularly polarized light.

[0016] P-polarized light is polarized light that vibrates parallel to the plane of incidence of the light. The plane of incidence is perpendicular to the reflecting surface (such as the surface of a windshield glass) and includes both the incident and reflected light rays. In p-polarized light, the vibration plane of the electric field vector is parallel to the plane of incidence.

[0017] The front retardation is a value measured using an AxoScan manufactured by Axometrics. Unless otherwise specified, the measurement wavelength is 550 nm. The front retardation can also be a value measured by irradiating light with a wavelength within the visible light wavelength range in the normal direction to the film using a KOBRA21ADH or WR (manufactured by Oji Scientific Instruments). The measurement wavelength can be selected by manually changing the wavelength selection filter or by converting the measured value using a program or the like.

[0018] "Projection image" means an image based on the projection of light from the projector used, rather than the surrounding scenery such as in front. A projection image is observed by an observer as a virtual image that appears to float beyond the projection image display portion of the laminated glass. "Screen image" means an image displayed on the projection device of the projector, or an image drawn by the drawing device on an intermediate image screen, etc. In contrast to a virtual image, a screen is a real image. Both the image and the projection image may be a monochromatic image, a multi-color image with two or more colors, or a full-color image.

[0019] The laminated glass of the present invention comprises a pair of glass plates, a luminescent layer containing a binder resin and a luminescent material including at least one selected from the group consisting of luminescent particles, luminescent pigments, and luminescent dyes, and a reflective layer. When the laminated glass of the present invention is applied to a windshield and an image display system, it is possible to display both so-called virtual images and real images. By combining a virtual image, which has a limited viewing angle, with a real image, which has no viewing angle limit, selective display is possible, for example, by displaying information that only the driver needs to see, such as the direction of travel, as a virtual image, and displaying information such as the time as a real image so that passengers can also see it.

[0020] The arrangement order of the pair of glass plates, the light-emitting layer, and the reflective layer is not particularly limited. FIG. 1 is a schematic diagram showing an example of the laminated glass of the present invention. The laminated glass 10 shown in FIG. 1 has, in this order, an outer glass 1, a light-emitting layer 2, an inner glass 3, and a reflective layer 4. FIG. 1 is also a schematic diagram showing an example of the laminated glass of the present invention. The laminated glass 11 shown in FIG. 2 has, in this order, an outer glass 1, an adhesive layer 5, a transparent resin substrate 6, a reflective layer 4, a light-emitting layer 2, and an inner glass 3. FIG. 3 is also a schematic diagram showing an example of the laminated glass of the present invention. The laminated glass 12 shown in FIG. 3 has, in this order, an outer glass 1, a light-emitting layer 2, a reflective layer 4, a transparent resin substrate 6, an adhesive layer 5, and an inner glass 3. FIG. 4 is also a schematic diagram showing an example of the laminated glass of the present invention. The laminated glass 13 shown in FIG. 4 has, in this order, an outer glass 1, a light-emitting layer 2, an inner glass 3, an adhesive layer 5, a reflective layer 4, a transparent resin substrate 6, and a hard coat layer 7. FIG. 5 is a schematic diagram showing an example of the laminated glass of the present invention. The laminated glass 13 shown in FIG. 5 has, in this order, an outer glass 1, a light-emitting layer 2, a retardation layer 9, a reflective layer 4, a polarization conversion layer 8, a transparent resin substrate 6, an adhesive layer 5, and an inner glass 3. FIG. 6 is a schematic diagram showing an example of the laminated glass of the present invention. The laminated glass 13 shown in FIG. 6 has, in this order, an outer glass 1, a light-emitting layer 2, an inner glass 3, an adhesive layer 5, a polarization conversion layer 8, a reflective layer 4, a retardation layer 9, a transparent resin substrate 6, and a hard coat layer 7. The inner glass is, for example, the glass located on the inner side of the vehicle when the laminated glass is applied to the vehicle, and the outer glass is, for example, the glass located on the outer side of the vehicle when the laminated glass is applied to the vehicle. Each component of the laminated glass will be described in detail below.

[0021] <Pair of Glass Plates> The glass plates constituting the pair of glass plates are not particularly limited and can be appropriately selected depending on the purpose. Examples of the glass plates include a transparent glass plate, a patterned glass plate, a wired glass plate, a reinforced glass plate, a heat-reflecting glass plate, a heat-absorbing glass plate, a Low-E glass plate, and various other glass plates.

[0022] The thickness of the glass plate is not particularly limited, and is preferably 1.8 to 6 mm. For example, standard float plate glass products manufactured by a float apparatus, such as those having a nominal thickness of 3 mm (commonly known as FL3), a nominal thickness of 4 mm (commonly known as FL4), a nominal thickness of 5 mm (commonly known as FL5), or a nominal thickness of 6 mm (commonly known as FL6), can be used.

[0023] <Light-emitting layer> The light-emitting layer contains a binder resin and a light-emitting material. By containing the light-emitting material, the light-emitting layer emits light when irradiated with light of a specific wavelength. By utilizing this property, information can be displayed with high contrast.

[0024] The binder resin is not particularly limited, and examples thereof include thermoplastic resins such as polyvinyl acetal resin, ethylene-vinyl acetate copolymer resin, ethylene-acrylic copolymer resin, polyurethane resin, polyurethane resin containing sulfur element, polyvinyl alcohol resin, vinyl chloride resin, and polyethylene terephthalate resin. Among these, polyvinyl acetal resin is preferred because it exhibits excellent adhesion to glass when used in combination with a plasticizer.

[0025] The polyvinyl acetal resin is not particularly limited as long as it is a polyvinyl acetal resin obtained by acetalizing polyvinyl alcohol with an aldehyde, but polyvinyl butyral resin is preferred. Furthermore, two or more polyvinyl acetal resins may be used in combination as needed. The degree of acetalization of the polyvinyl acetal resin is preferably 40 to 85 mol%, more preferably 60 to 75 mol%.

[0026] The hydroxyl group content of the polyvinyl acetal resin is preferably 15 to 35 mol %. A hydroxyl group content of 15 mol % or more is preferred because it improves adhesion between the light-emitting layer and glass. A hydroxyl group content of 35 mol % or less is preferred because it makes the light-emitting layer easier to handle. The acetalization degree and hydroxyl group content can be measured, for example, in accordance with JIS K6728 "Testing Methods for Polyvinyl Butyral."

[0027] As described above, polyvinyl acetal resins can be prepared by acetalizing polyvinyl alcohol with an aldehyde. The polyvinyl alcohol is typically obtained by saponifying polyvinyl acetate, and polyvinyl alcohol with a saponification degree of 70 to 99.8 mol% is commonly used. The saponification degree of the polyvinyl alcohol is preferably 80 to 99.8 mol%. The degree of polymerization of the polyvinyl alcohol is preferably 500 to 4000. When the degree of polymerization of the polyvinyl alcohol is 500 or more, the resulting laminated glass has high penetration resistance. When the degree of polymerization of the polyvinyl alcohol is 4000 or less, the interlayer film for laminated glass can be easily formed. The degree of polymerization of the polyvinyl alcohol is preferably 1000 to 3600.

[0028] The aldehyde is not particularly limited, but generally, an aldehyde having 1 to 10 carbon atoms is suitably used. The aldehyde having 1 to 10 carbon atoms is not particularly limited, and examples thereof include n-butylaldehyde, isobutyraldehyde, n-valeraldehyde, 2-ethylbutyraldehyde, n-hexylaldehyde, n-octylaldehyde, n-nonylaldehyde, n-decylaldehyde, formaldehyde, acetaldehyde, and benzaldehyde. Of these, n-butylaldehyde, n-hexylaldehyde, or n-valeraldehyde is preferred, and n-butylaldehyde is more preferred. These aldehydes may be used alone or in combination of two or more.

[0029] The luminescent material is at least one selected from the group consisting of luminescent particles, luminescent pigments, and luminescent dyes. The luminescent particles and the luminescent pigments are, for example, Y 2 O 2 S: Eu, BaMg 2 Al 16 O 27 :Eu, Mn, (SrCaBaMg) 5 (P.O. 4 ) 3 Cl: Eu, BaMg 2 Al 16 O 27 : Eu, BaMg 2 Al 16 O 27: Eu, Mn, Sr 5 (P.O. 4 ) 3 Cl: Eu, LaPO 4 :Ce, Tb, MgAl 11 O 19 : Ce, Tb, Y 2 O 3 :Eu, Y(PV)O 4 :Eu, 3.5MgO・0.5MgF 2 GeO 2 : Mn, Ca 10 (P.O. 4 ) 6 FCl: Sb, Mn, Sr 10 (P.O. 4 ) 6 FCl: Sb, Mn, (SrMg) 2 P 2 O 7 : Eu, Sr 2 P 2 O 7 : Eu, CaWO 4 , CaWO 4 : Pb, MgWO 4 , (BaCa) 5 (P.O. 4 ) 3 Cl:Eu, Sr 4 Al 14 O 25 : Eu, Zn 2 SiO 4 Examples of suitable phosphors include phosphors represented by the formula: ZnS, GaSe, SiC, CdTe, etc., or composites thereof, as well as particle-type phosphors such as ZnS particles, GaSe particles, SiC particles, and CdTe particles.

[0030] Examples of the luminescent dye include (carbazole-naphthalimide)-based dyes, (acetonitrile-triphenyleneamine)-based dyes, arylsulfonate cyanine dyes, perylene-based dyes, coumarin-based dyes, and tris(4,4,4-trifluoro-1-(2-thienyl)-1,3-butanedionate-O,O')bis(triphenylphosphine oxide-O-)europium.

[0031] Among the above-mentioned luminescent dyes, compounds having a naphthalimide skeleton or compounds having a coumarin skeleton are preferred. Compounds having a naphthalimide skeleton and compounds having a coumarin skeleton have high affinity for binder resins (preferably thermoplastic resins), and therefore can be uniformly dispersed in the binder resin, thereby obtaining a luminescent layer with high transparency and low haze. Furthermore, compounds having a naphthalimide skeleton and compounds having a coumarin skeleton have extremely excellent durability against ultraviolet light, and therefore a luminescent layer using these compounds can exhibit excellent light resistance.

[0032] Examples of the compound having a naphthalimide skeleton include 4-bromo-1,8-naphthalimide, 4-amino-1,8-naphthalimide, 4-methoxy-N-methylnaphthalimide, naphthalimide, 4-aminonaphthalimide, N-methyl-4-aminonaphthalimide, N-ethyl-4-aminonaphthalimide, N-propyl-4-aminonaphthalimide, N-n-butyl-4-aminonaphthalimide, 4-acetylaminonaphthalimide, N-methyl-4-acetylaminonaphthalimide, N-ethyl-4-acetylaminonaphthalimide, N-propyl-4-acetylaminonaphthalimide. N-butyl-4-acetylaminonaphthalimide, N-methyl-4-methoxynaphthalimide, N-ethyl-4-methoxynaphthalimide, N-propyl-4-methoxynaphthalimide, N-n-butyl-4-methoxynaphthalimide, N-methyl-4-ethoxynaphthalimide, N-ethyl-4-ethoxynaphthalimide, N-propyl-4-ethoxynaphthalimide, N-n-butyl-4-ethoxynaphthalimide, Lumogen FViolet 570 (trade name, manufactured by BASF Japan Ltd.), and Lumogen FBlue 650 (trade name, manufactured by BASF Japan Ltd.).

[0033] Examples of the compound having a coumarin skeleton include derivatives having an electron-donating substituent at the 7-position of the coumarin ring. More specifically, derivatives having an amino group at the 7-position of the coumarin ring include 3-(2'-benzothiazolyl)-7-diethylaminocoumarin (coumarin 6), 3-(2'-benzimidazolyl)-7-N,N-diethylaminocoumarin (coumarin 7), 3-(2'-N-methylbenzimidazolyl)-7-N,N-diethylaminocoumarin (coumarin 30), and 2,3,5,6-1H,4H-tetrahydro-8-trifluoromethylquinolizine(9,9a,1-gh)coumarin (coumarin 153). coumarin dyes such as phosphorus dyes and Basic Yellow 51, as well as 7-hydroxycoumarin, 3-cyano-7-hydroxycoumarin, 7-hydroxy-4-methylcoumarin, 7-diethylamino-4-methylcoumarin, 7-dimethylaminocyclopenta[c]-coumarin, 1,2,4,5,3H,6H,10H-tetrahydro-8-methyl[1]benzopyrano[9,9a,1-gH]quinolizin-10-one, 7-amino-4-trifluoromethylcoumarin, and the like, which are characterized by having a hydroxy group at the 7-position of the coumarin ring. coumarin, 1,2,4,5,3H,6H,10H-tetrahydro-9-cyano[1]benzopyrano[9,9a,1-gH]quinolizin-10-one, 1,2,4,5,3H,6H,10H-tetrahydro-9-carbo-t-butoxy[1]benzopyrano[9,9a,1-gH]quinolizin-10-one, 7-ethylamino-6-methyl-4-trifluoromethylcoumarin, 1,2,4,5,3H,6H,10H-tetrahydro-9-carbethoxy[1]benzopyrano[9,9a,1-gH]quinolizin-10-one, 7- Diethylamino-3-(1-methylbenzimidazolyl)coumarin, 7-dimethylamino-4-trifluoromethylcoumarin, 1,2,4,5,3H,6H,10H-tetrahydro-9-carboxy[1]benzopyrano[9,9a,1-gH]quinolizin-10-one, 1,2,4,5,3H,6H,10H-tetrahydro-9-acetyl[1]benzopyrano[9,9a,1-gH]quinolizin-10-one, 3-(2-benzimidazolyl)-7-N,N-diethylaminocoumarin, 1,2,4,5,3H,6H,Examples of the coumarin include 10H-tetrahydro-8-trifluoromethyl[1]benzopyrano[9,9a,1-gH]quinolizin-10-one, 3-(2-benzothiazolyl)-7-diethylaminocoumarin, 7-diethylaminocoumarin, 7-diethylamino-4-trifluoromethylcoumarin, 2,3,6,7-tetrahydro-9-(trifluoromethyl)-1H,5H,11H-[1]benzopyrano[6,7,8-ij]quinolizin-11-one, 7-amino-4-methylcoumarin, and 4,6-dimethyl-7-ethylaminocoumarin.

[0034] The above-mentioned light-emitting materials may be used alone or in combination of two or more. By combining multiple light-emitting materials that emit light of different wavelengths, it is possible to display not only monochromatic information but also information that combines various colors. In particular, by combining light-emitting materials that emit light of three colors (red, green, and blue) and controlling the wavelength of the emitted light to control the fluorescent wavelength, it is possible to display information in color.

[0035] The content of the luminescent material in the luminescent layer is preferably 0.005 to 5 parts by weight per 100 parts by weight of the binder resin. To achieve sufficient luminescence, it is preferable to incorporate a certain amount of luminescent material, but incorporating a large amount of luminescent material may actually reduce luminescence. This is thought to be due to the phenomenon of concentration quenching, in which the interaction of excited luminescent materials causes the absorbed energy to transition to a non-radiative process that does not emit light, thereby reducing the luminescence intensity. When the content of the luminescent material is within this range, luminescence with sufficiently high contrast can be obtained when irradiated with light of a specific wavelength. The content of the luminescent material is preferably 0.01 to 3 parts by weight, more preferably 0.05 to 1 part by weight, per 100 parts by weight of the binder resin.

[0036] The content of the light-emitting material in the light-emitting layer is preferably 0.005 to 5% by mass, based on 100% by mass of the light-emitting layer. When the content of the light-emitting material is 0.005% by mass or more, a light-emitting layer capable of displaying images with even higher contrast can be obtained. When the content of the light-emitting material is 5% by mass or less, a light-emitting layer having even higher transparency can be obtained. The content of the light-emitting material is preferably 0.01 to 3% by mass, more preferably 0.02 to 1% by mass, based on 100% by mass of the light-emitting layer.

[0037] The light-emitting layer preferably further contains a dispersant. By including a dispersant, the light-emitting material can be finely dispersed in the light-emitting layer, enabling more uniform light emission. Examples of the dispersant include compounds having a sulfonic acid structure such as linear alkylbenzene sulfonate, compounds having an ester structure such as diester compounds, alkyl ricinoleate esters, phthalates, adipates, sebacates, and phosphates, compounds having an ether structure such as polyoxyethylene glycol, polyoxypropylene glycol, and alkylphenyl-polyoxyethylene-ether, compounds having a carboxylic acid structure such as polycarboxylic acids, compounds having an amine structure such as laurylamine, dimethyllaurylamine, oleylpropylenediamine, secondary amines of polyoxyethylene, tertiary amines of polyoxyethylene, and diamines of polyoxyethylene, compounds having a polyamine structure such as polyalkylenepolyamine alkylene oxide, and the like. Examples of suitable dispersants include compounds having an amide structure such as leic acid diethanolamide and alkanol fatty acid amide, compounds having a high molecular weight amide structure such as polyvinylpyrrolidone and polyester acid amide amine salt, compounds having a silane structure with an alkyl group such as triethoxypropyl isocyanate silane and triethoxybutyl silane, compounds having a silane structure with an acryloxy group such as triethoxypropyl acryloxysilane, compounds having a silane structure with a vinyl group such as triethoxypropyl vinyl silane, compounds having a high molecular weight polysiloxane structure with side chains such as epoxy groups, phosphate groups, carboxyl groups, and mercapto groups, compounds having an isocyanate group such as isocyanate, and compounds having an isocyanurate group such as isocyanurate. Examples of suitable dispersants include high molecular weight dispersants such as polyoxyethylene alkyl ether phosphate (salt), polymeric polycarboxylic acid, and condensed ricinoleic acid ester. A high molecular weight dispersant is defined as a dispersant with a molecular weight of 10,000 or more.

[0038] When the dispersant is added, the amount of the dispersant added to the light-emitting layer is preferably 1 to 50 parts by mass per 100 parts by weight of the light-emitting material. When the amount of the dispersant added is within this range, the light-emitting material can be uniformly dispersed in the light-emitting layer. The amount of the dispersant added is preferably 3 to 30 parts by mass, and more preferably 5 to 25 parts by mass.

[0039] The light-emitting layer preferably further contains an ultraviolet absorber. The light-emitting material tends to deteriorate due to long-term exposure to ultraviolet light, resulting in a decrease in light-emitting performance. When the light-emitting layer contains an ultraviolet absorber, deterioration of the light-emitting material due to ultraviolet light can be suppressed. The light-emitting layer does not necessarily contain an ultraviolet absorber. Since a light-emitting layer capable of displaying images with even higher contrast can be obtained, the content of the ultraviolet absorber in the light-emitting layer is preferably 1 part by mass or less, more preferably 0.5 parts by mass or less, even more preferably 0.2 parts by mass or less, particularly preferably 0.1 parts by mass or less, and preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, relative to 100 parts by mass of the binder resin.

[0040] Examples of the ultraviolet absorber include conventionally known ultraviolet absorbers such as compounds having a malonic acid ester structure, compounds having an oxalic acid anilide structure, compounds having a benzotriazole structure, compounds having a benzophenone structure, compounds having a triazine structure, compounds having a benzoate structure, and compounds having a hindered amine structure.

[0041] The light-emitting layer may further contain a plasticizer, if necessary. The plasticizer is not particularly limited, and examples thereof include organic ester plasticizers such as monobasic organic acid esters and polybasic organic acid esters, and phosphate plasticizers such as organic phosphate plasticizers and organic phosphite plasticizers. The plasticizer is preferably a liquid plasticizer.

[0042] The monobasic organic acid ester is not particularly limited, and examples thereof include glycol esters obtained by reacting glycols such as triethylene glycol, tetraethylene glycol, and tripropylene glycol with monobasic organic acids such as butyric acid, isobutyric acid, caproic acid, 2-ethylbutyric acid, heptyl acid, n-octylic acid, 2-ethylhexylic acid, pelargonic acid (n-nonylic acid), and decylic acid. Of these, triethylene glycol dicaproic acid ester, triethylene glycol di-2-ethylbutyric acid ester, triethylene glycol di-n-octylic acid ester, and triethylene glycol di-2-ethylhexylic acid ester are preferred.

[0043] The polybasic organic acid ester is not particularly limited, but examples thereof include ester compounds of polybasic organic acids such as adipic acid, sebacic acid, and azelaic acid with alcohols having a linear or branched structure and having 4 to 8 carbon atoms. Among these, dibutyl sebacate, dioctyl azelate, and dibutyl carbitol adipate are preferred.

[0044] The organic ester plasticizer is not particularly limited, and examples thereof include triethylene glycol di-2-ethylbutyrate, triethylene glycol di-2-ethylhexanoate, triethylene glycol dicaprylate, triethylene glycol di-n-octanoate, triethylene glycol di-n-heptanoate, tetraethylene glycol di-n-heptanoate, tetraethylene glycol di-2-ethylhexanoate, dibutyl sebacate, dioctyl azelate, dibutyl carbitol adipate, ethylene glycol di-2-ethylbutyrate, 1,3-propylene glycol di-2-ethylbutyrate, 1,4-butylene glycol di-2-ethylbutyrate, diethylene ... Examples of the adipate include ethylene glycol di-2-ethylhexanoate, dipropylene glycol di-2-ethylbutyrate, triethylene glycol di-2-ethylpentanoate, tetraethylene glycol di-2-ethylbutyrate, diethylene glycol dicaprylate, dihexyl adipate, dioctyl adipate, hexylcyclohexyl adipate, diisononyl adipate, heptylnonyl adipate, dibutyl sebacate, oil-modified alkyd sebacate, a mixture of a phosphate ester and an adipate ester, an adipate, a mixed adipate prepared from an alkyl alcohol having 4 to 9 carbon atoms and a cyclic alcohol having 4 to 9 carbon atoms, and an adipate having 6 to 8 carbon atoms such as hexyl adipate.

[0045] The organic phosphoric acid plasticizer is not particularly limited, and examples thereof include tributoxyethyl phosphate, isodecylphenyl phosphate, and triisopropyl phosphate.

[0046] Among the above plasticizers, by using at least one selected from the group consisting of dihexyl adipate (DHA), triethylene glycol di-2-ethylhexanoate (3GO), tetraethylene glycol di-2-ethylhexanoate (4GO), triethylene glycol di-2-ethylbutyrate (3GH), tetraethylene glycol di-2-ethylbutyrate (4GH), tetraethylene glycol di-n-heptanoate (4G7), and triethylene glycol di-n-heptanoate (3G7), it is possible to prevent deterioration over time in the adhesive strength to glass when the light-emitting layer is used as an interlayer film for laminated glass.

[0047] Furthermore, the plasticizer preferably contains triethylene glycol di-2-ethylhexanoate (3GO), triethylene glycol di-2-ethylbutyrate (3GH), tetraethylene glycol di-2-ethylhexanoate (4GO), or dihexyl adipate (DHA) because they are less susceptible to hydrolysis, with tetraethylene glycol di-2-ethylhexanoate (4GO) or triethylene glycol di-2-ethylhexanoate (3GO) being preferred, and triethylene glycol di-2-ethylhexanoate being more preferred.

[0048] The content of the plasticizer in the light-emitting layer is not particularly limited, but is preferably 30 to 80 parts by mass relative to 100 parts by mass of the binder resin. When the content of the plasticizer is 30 parts by mass or more, the melt viscosity of the light-emitting layer is reduced, and degassing properties are improved when the light-emitting layer is used as an interlayer film for laminated glass to produce laminated glass. When the content of the plasticizer is 80 parts by mass or less, the transparency of the light-emitting layer is increased. The content of the plasticizer is more preferably 35 parts by mass or more, more preferably 70 parts by mass or less, and even more preferably 63 parts by mass.

[0049] The light-emitting layer may contain additives such as antioxidants, light stabilizers, antistatic agents, adhesion modifiers, blue pigments, blue dyes, green pigments, and green dyes, as needed.

[0050] The light-emitting layer preferably contains an antioxidant, as this allows for excellent light resistance to be obtained. The antioxidant is not particularly limited, and examples include antioxidants having a phenol structure, antioxidants containing sulfur, and antioxidants containing phosphorus. The antioxidants may be used alone or in combination of two or more. The antioxidant having a phenol structure is an antioxidant having a phenol skeleton. Examples of the antioxidant having a phenol structure include 2,6-di-t-butyl-p-cresol (BHT), butylated hydroxyanisole (BHA), 2,6-di-t-butyl-4-ethylphenol, stearyl-β-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2,2'-methylenebis-(4-methyl-6-butylphenol), 2,2'-methylenebis-(4-ethyl-6-t-butylphenol), 4,4'-butylidene-bis-(3-methyl-6-t-butylphenol), 1,1,3-tris-(2-methyl-hydroxy- 5-t-butylphenyl)butane, tetrakis[methylene-3-(3',5'-butyl-4-hydroxyphenyl)propionate]methane, 1,3,3-tris-(2-methyl-4-hydroxy-5-t-butylphenol)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, bis(3,3'-t-butylphenol)butylic acid glycol ester, and pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate].

[0051] The light-emitting layer preferably contains the adhesion modifier. The adhesion modifier is not particularly limited, but is preferably a metal salt, and more preferably at least one metal salt selected from the group consisting of alkali metal salts, alkaline earth metal salts, and Mg salts. The metal salt preferably contains at least one metal selected from the group consisting of K and Mg. The metal salt is more preferably an alkali metal salt of an organic acid having 2 to 16 carbon atoms or an alkaline earth metal salt of an organic acid having 2 to 16 carbon atoms, and even more preferably a magnesium salt of a carboxylic acid having 2 to 16 carbon atoms or a potassium salt of a carboxylic acid having 2 to 16 carbon atoms. The magnesium salt of a carboxylic acid having 2 to 16 carbon atoms and the potassium salt of a carboxylic acid having 2 to 16 carbon atoms are not particularly limited, but examples thereof include magnesium acetate, potassium acetate, magnesium propionate, potassium propionate, magnesium 2-ethylbutanoate, potassium 2-ethylbutanoate, magnesium 2-ethylhexanoate, and potassium 2-ethylhexanoate.

[0052] The content of the adhesion modifier is not particularly limited, but is preferably 0.0005 to 0.05 parts by mass relative to 100 parts by mass of the binder resin. When the content of the adhesion modifier is 0.0005 parts by mass or more, the penetration resistance of the laminated glass is increased. When the content of the adhesion modifier is 0.05 parts by mass or less, the transparency of the light-emitting layer is increased. The content of the adhesion modifier is preferably 0.002 to 0.02 parts by mass relative to 100 parts by mass of the binder resin.

[0053] The thickness of the light-emitting layer is not particularly limited, but is preferably 50 to 1000 μm. When the thickness of the light-emitting layer is within this range, light emission with sufficiently high contrast can be obtained when irradiated with light of a specific wavelength, and the light-emitting layer is also suitable for applications such as an interlayer film for laminated glass. The thickness of the light-emitting layer is more preferably 100 to 800 μm.

[0054] The light-emitting layer may be disposed on the entire horizontal surface of the laminated glass of the present invention, or may be disposed on only a portion thereof. When the light-emitting layer is disposed on only a portion thereof, the portion may be made a light-emitting area and the other portion a non-light-emitting area, so that information can be displayed only in the light-emitting area.

[0055] The light-emitting layer preferably has a first resin layer containing a binder resin disposed on one surface of the light-emitting layer, and more preferably is laminated so that the light-emitting layer and the first resin layer are in contact with each other. Furthermore, it is preferable that a second resin layer containing a binder resin is disposed on the surface of the light-emitting layer opposite to the surface on which the first resin layer is disposed, and more preferably is laminated so that the light-emitting layer and the second resin layer are in contact with each other. That is, it is preferable that the first resin layer, the light-emitting layer, and the second resin layer are disposed in this order.

[0056] The first resin layer and the second resin layer may contain a polyvinyl acetal resin, a plasticizer, an adhesion modifier, and an ultraviolet absorber. The polyvinyl acetal resin, plasticizer, adhesion modifier, and ultraviolet absorber contained in the first resin layer and the second resin layer may be the same as the polyvinyl acetal resin, plasticizer, adhesion modifier, and ultraviolet absorber used in the light-emitting layer. The first resin layer and the second resin layer may also contain the light-emitting material. In this case, the content of the light-emitting material in the first resin layer and the second resin layer per 100 parts by mass of the binder resin is preferably less than the content of the light-emitting material in the light-emitting layer per 100 parts by mass of the binder resin in the light-emitting layer.

[0057] As described above, the luminescent material contained in the luminescent layer tends to deteriorate due to long-term irradiation with ultraviolet light, resulting in a decrease in luminescent performance. By laminating the first resin layer and the second resin layer containing an ultraviolet absorber on the luminescent layer, it is possible to prevent the deterioration of the luminescent material due to ultraviolet light.

[0058] When the light-emitting layer is required to have heat-shielding properties, at least one of the light-emitting layer, the first resin layer, and the second resin layer may contain a heat-ray absorbing agent, or a heat-ray shielding layer containing a binder resin and a heat-ray absorbing agent may be laminated on the light-emitting layer, the first resin layer, and the second resin layer.

[0059] The heat ray absorber is not particularly limited as long as it has the ability to shield infrared rays, but at least one selected from the group consisting of tin-doped indium oxide (ITO) particles, antimony-doped tin oxide (ATO) particles, aluminum-doped zinc oxide (AZO) particles, indium-doped zinc oxide (IZO) particles, tin-doped zinc oxide particles, silicon-doped zinc oxide particles, lanthanum hexaboride particles, and cerium hexaboride particles is suitable.

[0060] The light-emitting layer may further include a sound-insulating layer for the purpose of improving sound-insulating performance. Examples of the sound-insulating layer include a layer containing 50 parts by mass or more of the plasticizer per 100 parts by mass of the binder resin. Adjusting the amount of plasticizer contained in any of the light-emitting layer, the first resin layer, the second resin layer, and the heat-shielding layer can also serve as a sound-insulating layer. The binder resin contained in the sound-insulating layer is preferably a thermoplastic resin, more preferably a polyvinyl acetal resin. The polyvinyl acetal resin contained in the sound-insulating layer preferably has a hydroxyl group content of less than 28 mol%. The polyvinyl acetal resin contained in the sound-insulating layer may be polyvinyl acetal resin A having an acetyl group content of 8 mol% or more, polyvinyl acetal resin B having an acetyl group content of less than 5 mol% and an acetalization degree of 70 mol% or more, or polyvinyl acetal resin C having an acetyl group content of 5 mol% or more but less than 8 mol% and an acetalization degree of 65 mol% or more.

[0061] The light-emitting layer, the first resin layer, and the second resin layer each contain a polyvinyl acetal resin and a plasticizer, and the content of the plasticizer per 100 parts by mass of the polyvinyl acetal resin in the light-emitting layer (hereinafter also referred to as content A) is preferably greater than the content of the plasticizer per 100 parts by mass of the polyvinyl acetal resin in the first resin layer and the second resin layer (hereinafter also referred to as content B). When content A is greater than content B, the sound insulation of the light-emitting layer can be further improved. Content A is preferably 5 parts by mass or more greater than content B, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more.

[0062] When the first resin layer and the second resin layer are laminated on the light-emitting layer, it is preferable to prevent the light-emitting material contained in the light-emitting layer from migrating to the first resin layer and the second resin layer in order to display an image with even higher contrast. Examples of methods for preventing the light-emitting material contained in the light-emitting layer from migrating to the first resin layer and the second resin layer include a method (Method 1) in which the compatibility between the binder resin contained in the light-emitting layer and the light-emitting material is made higher than the compatibility between the binder resin contained in the first resin layer and the second resin layer and the light-emitting material. Furthermore, when the light-emitting layer and the first and second resin layers contain a binder resin and a plasticizer, examples of methods include a method (Method 2) in which the compatibility between the plasticizer contained in the light-emitting layer and the light-emitting material is made higher than the compatibility between the plasticizer contained in the first and second resin layers and the fluorescent material, and a method (Method 3) in which the plasticizer contained in the light-emitting layer is prevented from migrating to the first and second resin layers. It is believed that when the plasticizer contained in the light-emitting layer migrates to the first resin layer and the second resin layer, the light-emitting material migrates along with the plasticizer. Note that compatibility refers to the ease with which components mix, which is different from compatibility.

[0063] Methods 1 to 3 will be described in more detail below for a case where the first resin layer, the light-emitting layer, and the second resin layer are laminated in this order, and the light-emitting layer, the first resin layer, and the second resin layer contain a polyvinyl acetal resin and a plasticizer.

[0064] In the above method 1, the compatibility between the polyvinyl acetal resin and the light-emitting material can be appropriately set by adjusting the amount of hydroxyl groups in the polyvinyl acetal resin. When the light-emitting material is hydrophobic, the amount of hydroxyl groups in the polyvinyl acetal resin contained in the light-emitting layer is preferably lower than the amount of hydroxyl groups in the polyvinyl acetal resin contained in the first resin layer and the second resin layer. When the light-emitting material is hydrophilic, the amount of hydroxyl groups in the polyvinyl acetal resin contained in the light-emitting layer is preferably higher than the amount of hydroxyl groups in the polyvinyl acetal resin contained in the first resin layer and the second resin layer. The absolute value of the difference between the amount of hydroxyl groups in the polyvinyl acetal resin contained in the light-emitting layer and the amount of hydroxyl groups in the polyvinyl acetal resin contained in the first resin layer and the second resin layer is preferably 1 to 20 mol%, more preferably 3 to 15 mol%, and even more preferably 5 to 10 mol%.

[0065] In the method 2, the compatibility between the plasticizer and the light-emitting material can be appropriately adjusted by adjusting the plasticizer contained in the light-emitting layer and the first and second resin layers. For example, it is preferable that the plasticizer contained in the light-emitting layer is different from the plasticizer contained in the first and second resin layers, and that the compatibility between the plasticizer contained in the light-emitting layer and the light-emitting material is higher than the compatibility between the plasticizer contained in the first and second resin layers and the light-emitting material. When the light-emitting material is hydrophobic, it is preferable that the plasticizer contained in the light-emitting layer is more hydrophobic than the plasticizer contained in the first and second resin layers. When the light-emitting material is hydrophilic, it is preferable that the plasticizer contained in the light-emitting layer is more hydrophilic than the plasticizer contained in the first and second resin layers.

[0066] In the above method 3, the migration of the plasticizer can be appropriately controlled by adjusting the amount of hydroxyl groups in the polyvinyl acetal resin contained in the light-emitting layer and the first and second resin layers. To prevent migration of the plasticizer, the amount of hydroxyl groups in the polyvinyl acetal resin contained in the light-emitting layer is preferably lower than the amount of hydroxyl groups in the polyvinyl acetal resin contained in the first and second resin layers. In particular, when the plasticizer is hydrophobic, migration of the plasticizer contained in the light-emitting layer to the first and second resin layers can be suppressed, resulting in a light-emitting layer capable of displaying images with even higher contrast. The amount of hydroxyl groups in the polyvinyl acetal resin contained in the light-emitting layer is preferably at least 1 mol% lower, more preferably at least 3 mol%, even more preferably at least 5 mol%, and particularly preferably at least 7 mol% lower than the amount of hydroxyl groups in the polyvinyl acetal resin contained in the first and second resin layers. The difference between the amount of hydroxyl groups in the polyvinyl acetal resin contained in the light-emitting layer and the amount of hydroxyl groups in the polyvinyl acetal resin contained in the first resin layer and the second resin layer is preferably 20 mol % or less, more preferably 15 mol % or less, and even more preferably 10 mol % or less.

[0067] <Reflective Layer> The reflective layer is not particularly limited as long as it is a layer that reflects light, and may be, for example, a layer including a dielectric layer and a metal layer, or a cholesteric liquid crystal layer having a selective reflection center wavelength in a specific wavelength range. A reflective layer having a low reflectance at an incident angle of 0° is preferred because it increases the transmittance of the windshield glass. A high reflectance at an incident angle of 65° is preferred because it increases the visibility of the projected image.

[0068] When the reflective layer is a reflective layer that selectively reflects light in a wavelength range, the reflective layer may include a cholesteric liquid crystal layer having a selective reflection center wavelength in the red wavelength range, a cholesteric liquid crystal layer having a selective reflection center wavelength in the green wavelength range, and a cholesteric liquid crystal layer having a selective reflection center wavelength in the blue wavelength range. The three cholesteric liquid crystal layers have different selective reflection center wavelengths. Each cholesteric liquid crystal layer may be in direct contact with any of the other cholesteric liquid crystal layers.

[0069] As is well known, a cholesteric liquid crystal layer is a layer in which liquid crystal compounds are fixed in a helical oriented state of a cholesteric liquid crystal phase, and reflects light with a selective reflection center wavelength corresponding to the pitch of the helical structure and transmits light in other wavelength ranges. Furthermore, a cholesteric liquid crystal layer exhibits selective reflection for either left- or right-handed circularly polarized light at a specific wavelength.

[0070] Here, it is preferable from the viewpoint of visibility that the reflective layer having a cholesteric liquid crystal layer satisfy the following requirements (i) to (iii): (i) in the wavelength range of 400 nm or more and less than 500 nm, the maximum value of natural light reflectance is 10 to 35%, the difference between the maximum and minimum values ​​of natural light reflectance is 3% or more, and the total value of the wavelength bandwidth of the region higher than the average value of the maximum and minimum values ​​of natural light reflectance is 20 to 80 nm; (ii) in the wavelength range of 500 nm or more and less than 600 nm, the maximum value of natural light reflectance is 10 to 35%, the difference between the maximum and minimum values ​​of natural light reflectance is 3% or more, and the total value of the wavelength bandwidth of the region higher than the average value of the maximum and minimum values ​​of natural light reflectance is 20 to 80 nm. (iii) In the wavelength range of 600 to 800 nm, the maximum value of the natural light reflectance is 10 to 35%, and the total value of the wavelength bandwidth of the region higher than the average value of the maximum and minimum values ​​of the natural light reflectance is 120 nm or more.

[0071] In a reflective layer having a cholesteric liquid crystal layer, the reflected wavelength and reflectance can be adjusted by the selective reflection center wavelength, thickness (helical pitch number) of the cholesteric liquid crystal layer, etc. Reflection that satisfies requirement (i) can be realized mainly by a cholesteric liquid crystal layer that reflects light in the blue wavelength region, reflection that satisfies requirement (ii) can be realized by a cholesteric liquid crystal layer that reflects light in the green wavelength region, and reflection that satisfies requirement (iii) can be realized by a cholesteric liquid crystal layer that reflects light in the red wavelength region.

[0072] From the viewpoint of increasing transmittance while improving reflected color, the maximum natural light reflectance at 400 nm or more and less than 500 nm is preferably 11 to 35%, more preferably 12 to 30%. Similarly, from the viewpoint of increasing transmittance while improving reflected color, the maximum natural light reflectance at 500 nm or more and less than 600 nm is preferably 11 to 35%, more preferably 12 to 30%. From the viewpoint of increasing brightness of a displayed image while improving reflected color, the maximum natural light reflectance at 600 to 800 nm is preferably 15 to 35%, more preferably 16 to 30%.

[0073] From the viewpoint of being able to increase transmittance while improving reflected color, the difference between the maximum and minimum natural light reflectance values ​​at wavelengths of 400 nm or more and less than 500 nm is preferably 4 to 20%, more preferably 4 to 12%. Similarly, from the viewpoint of being able to increase transmittance while improving reflected color, the difference between the maximum and minimum natural light reflectance values ​​at wavelengths of 500 nm or more and less than 600 nm is preferably 4 to 20%, more preferably 4 to 12%.

[0074] From the viewpoint of being able to increase transmittance while improving reflected color, the wavelength bandwidth of the region where the reflectance is higher than the average of the maximum and minimum values ​​of the reflectance at 400 nm or more and less than 500 nm is preferably 30 to 78 nm, more preferably 35 to 75 nm. Similarly, from the viewpoint of being able to increase transmittance while improving reflected color, the wavelength bandwidth of the region where the reflectance is higher than the average of the maximum and minimum values ​​of the reflectance at 500 nm or more and less than 600 nm is preferably 30 to 78 nm, more preferably 35 to 75 nm. The narrower the wavelength bandwidth at 400 nm or more and less than 500 nm and the narrower the wavelength bandwidth at 500 nm or more and less than 600 nm, the more advantageous the transmittance is. However, since the wavelength bandwidth at 600 to 800 nm is wide, if the wavelength bandwidth at 400 nm or more and less than 500 nm and / or the wavelength bandwidth at 500 nm or more and less than 600 nm is too narrow, the reflected color may deteriorate. From this point of view, it is preferable that the wavelength bandwidth from 400 nm to less than 500 nm and the wavelength bandwidth from 500 nm to less than 600 nm are within the above ranges. Furthermore, the wavelength bandwidth from 500 nm to less than 600 nm has a greater effect on the transmittance.

[0075] From the viewpoint of improving the reflected color and the front brightness of the displayed image, the wavelength bandwidth of the region in which the reflectance is higher than the average value of the maximum and minimum values ​​of the reflectance in the range of 600 to 800 nm is preferably 120 to 200 nm.

[0076] The reflective layer having a cholesteric liquid crystal layer preferably has two or more cholesteric liquid crystal layers having different selective reflection center wavelengths, and each cholesteric liquid crystal layer is preferably in direct contact with any other cholesteric liquid crystal layer.

[0077] If the cholesteric liquid crystal layers are spaced apart, the thickness between the layers becomes thicker, making it difficult to obtain the effect of interference of light reflected by each cholesteric liquid crystal layer. In contrast, a configuration in which the cholesteric liquid crystal layers are in contact with each other is preferable because the wavelength band width can be narrowed by the effect of interference of light reflected by each cholesteric liquid crystal layer. In particular, if the thickness of each cholesteric liquid crystal layer is thinner than the wavelength of light (visible light 380 to 780 nm), the effect of interference becomes more pronounced, which is preferable.

[0078] In the present invention, when the reflective layer has two or more cholesteric liquid crystal layers, the cholesteric liquid crystal layers are not limited to being in direct contact with each other, and may be laminated via an adhesive layer or the like.

[0079] Here, each cholesteric liquid crystal layer may have at least one selective reflection center wavelength, but at least one of the cholesteric liquid crystal layers may have two or more selective reflection center wavelengths. A cholesteric liquid crystal layer having two or more selective reflection center wavelengths is achieved by a helical structure in which the helical pitch changes in the thickness direction.

[0080] The total thickness of the reflective layer including the cholesteric liquid crystal layer is preferably 0.4 to 2.0 μm, more preferably 0.6 to 1.8 μm, and even more preferably 0.8 to 1.4 μm. If the total thickness of the reflective layer is too thin, the natural light reflectance of the reflective layer may be too low, making it difficult to increase the brightness of the displayed image. On the other hand, if the total thickness of the reflective layer is too thick, the transmittance may be reduced.

[0081] Here, the laminated glass of the present invention preferably reflects linearly polarized light. When a reflective layer is incorporated into the laminated glass and used as a combiner for a head-up display, the projected image light is preferably p-polarized, i.e., linearly polarized light, in order to suppress reflection on the laminated glass surface. On the other hand, in the present invention, the reflective layer has a cholesteric liquid crystal layer and reflects circularly polarized light. Therefore, the laminated glass of the present invention preferably has a layer that converts linearly polarized light incident on the reflection into circularly polarized light. Examples of layers that convert the polarization state of light include a polarization conversion layer and a retardation layer.

[0082] The polarization conversion layer exhibits optical rotation and birefringence for visible light and converts the polarization state of incident light. In the present invention, the polarization conversion layer is made of a layer in which a birefringent material such as a liquid crystal compound is oriented with a twist of 360° or less. The retardation layer imparts a phase difference (optical path difference) to two orthogonal polarized light components to change the state of incident polarized light. In the present invention, the retardation layer is a layer in which a birefringent material such as a liquid crystal compound is oriented in the same direction and does not have optical rotation.

[0083] By configuring the laminated glass to have a polarization conversion layer or a retardation layer on the side of the reflective layer where light is incident, linearly polarized light incident on the laminated glass can be converted into circularly polarized light, the reflective layer can reflect the circularly polarized light, and the polarization conversion layer or retardation layer can convert the reflected circularly polarized light into linearly polarized light before it exits.

[0084] 5, the laminated glass 14 has a polarization conversion layer 8 on one side of the reflective layer 4 and a retardation layer 9 on the other side. When such a configuration is incorporated into the laminated glass, the polarization conversion layer 8 is disposed on the inner glass 3 side, which faces the vehicle interior, as shown in FIG. 5, which will be described later, for example.

[0085] In this case, the polarization conversion layer 8 functions to convert projected p-polarized light (linearly polarized light) into circularly polarized light reflected by the cholesteric liquid crystal layer of the reflective layer 4. Meanwhile, the retardation layer 9 functions to provide optical compensation for light incident from outside the laminated glass. For example, the polarization state of s-polarized light incident from outside the laminated glass changes when passing through the polarization conversion layer 8, resulting in the mixing of p-polarized light components. Because polarized sunglasses filter s-polarized light, this p-polarized light component passes through the polarized sunglasses. This impairs the polarized sunglasses' ability to filter glare from reflected light, which is primarily s-polarized light, and can cause problems while driving. In response to this problem, the inclusion of the retardation layer 9 and the optical compensation provided by the retardation layer 9 can improve the suitability for polarized sunglasses.

[0086] 5, the laminated glass 14 is configured so that the polarization conversion layer 8 faces the inner glass 3, but this is not limitative. The retardation layer 9 may also be configured so that it faces the inner glass 3.

[0087] In this case, the retardation layer 9 has the function of converting projected p-polarized light (linearly polarized light) into circularly polarized light that is reflected by the cholesteric liquid crystal layer of the reflective layer 4. On the other hand, the polarization conversion layer 8 has the function of optically compensating for light that enters from the outside of the laminated glass, and optical compensation by the polarization conversion layer 8 can improve suitability for polarized sunglasses.

[0088] The laminated glass of the present invention may have a polarization conversion layer on both sides of the reflective layer 4, or a retardation layer on both sides. In this case, the polarization conversion layer or retardation layer placed on the inner glass may have a function of converting projected p-polarized light (linearly polarized light) into circularly polarized light reflected by the cholesteric liquid crystal layer of the reflective layer 4. On the other hand, the polarization conversion layer or retardation layer placed on the outer glass may have a function of optically compensating for light incident from outside the laminated glass. Polarization conversion layers and retardation layers will be described in detail later.

[0089] (Method for producing a cholesteric liquid crystal layer) Hereinafter, the materials and method for producing a cholesteric liquid crystal layer will be described. Examples of materials used to form the above-mentioned cholesteric liquid crystal layer include a liquid crystal composition containing a polymerizable liquid crystal compound and a chiral agent (optically active compound). If necessary, the above-mentioned liquid crystal composition may be further mixed with a surfactant, a polymerization initiator, etc., and dissolved in a solvent, etc., and applied to a support, an alignment layer, a cholesteric liquid crystal layer that will be the underlying layer, etc., and after cholesteric alignment maturation, the liquid crystal composition may be cured and fixed to form a cholesteric liquid crystal layer.

[0090] (Polymerizable Liquid Crystal Compound) The polymerizable liquid crystal compound may be a rod-shaped liquid crystal compound or a discotic liquid crystal compound, but is preferably a rod-shaped liquid crystal compound. Examples of rod-shaped polymerizable liquid crystal compounds that form a cholesteric liquid crystal layer include rod-shaped nematic liquid crystal compounds. Preferred rod-shaped nematic liquid crystal compounds include azomethines, azoxys, cyanobiphenyls, cyanophenyl esters, benzoic acid esters, cyclohexanecarboxylic acid phenyl esters, cyanophenylcyclohexanes, cyano-substituted phenylpyrimidines, alkoxy-substituted phenylpyrimidines, phenyldioxanes, tolanes, and alkenylcyclohexylbenzonitriles. Not only low-molecular-weight liquid crystal compounds but also polymer-molecular-weight liquid crystal compounds can be used.

[0091] A polymerizable liquid crystal compound can be obtained by introducing a polymerizable group into a liquid crystal compound. Examples of the polymerizable group include an unsaturated polymerizable group, an epoxy group, and an aziridinyl group, with an unsaturated polymerizable group being preferred, and an ethylenically unsaturated polymerizable group being more preferred. The polymerizable group can be introduced into the molecule of the liquid crystal compound by various methods. The number of polymerizable groups contained in the polymerizable liquid crystal compound is preferably 1 to 6, more preferably 1 to 3, per molecule. Examples of polymerizable liquid crystal compounds are described in Makromol. Chem. , Vol. 190, p. 2255 (1989), Advanced Materials Vol. 5, p. 107 (1993), U.S. Pat. No. 4,683,327, U.S. Pat. No. 5,622,648, U.S. Pat. No. 5,770,107, WO95 / 022586, WO95 / 024455, WO97 / 000600, WO98 / 023580, WO98 / 052905, JP-A Nos. 1-272551, 6-016616, 7-110469, 11-080081, and 2001-0328973. Two or more polymerizable liquid crystal compounds may be used in combination. The use of two or more polymerizable liquid crystal compounds in combination can lower the alignment temperature.

[0092] Further, a specific example of the polymerizable liquid crystal compound is the following mixture 1.

[0093]

[0094] The amount of the polymerizable liquid crystal compound added in the liquid crystal composition is preferably 80 to 99.9 mass %, more preferably 85 to 99.5 mass %, and even more preferably 90 to 99 mass %, based on the solid content mass (mass excluding the solvent) of the liquid crystal composition.

[0095] In order to improve the visible light transmittance, the cholesteric liquid crystal layer may have a low Δn. The low Δn cholesteric liquid crystal layer can be formed using a low Δn polymerizable liquid crystal compound. The low Δn polymerizable liquid crystal compound will be specifically described below.

[0096] (Low Δn polymerizable liquid crystal compound) A cholesteric liquid crystal phase is formed using a low Δn polymerizable liquid crystal compound, and this is fixed into a film, thereby obtaining a narrow-band reflective layer. Examples of low Δn polymerizable liquid crystal compounds include the compounds described in WO2015 / 115390, WO2015 / 147243, WO2016 / 035873, JP2015-163596A, and JP2016-053149A. For liquid crystal compositions that provide reflective layers with small half-widths, the description in WO2016 / 047648 can also be referenced.

[0097] The liquid crystal compound is also preferably a polymerizable compound represented by the following formula (I) described in WO2016 / 047648.

[0098]

[0099] In formula (I), A represents a phenylene group which may have a substituent or a trans-1,4-cyclohexylene group which may have a substituent; L represents a linking group selected from the group consisting of a single bond, —CHO—, —OCH—, —(CH)OC(═O)—, —C(═O)O(CH)—, —C(═O)O—, —OC(═O)—, —OC(═O)O—, —CH═CH—C(═O)O—, and —OC(═O)—CH═CH—; m represents an integer of 3 to 12; Sp 1 and Sp 2each independently represents a linking group selected from the group consisting of a single bond, a linear or branched alkylene group having 1 to 20 carbon atoms, and a linear or branched alkylene group having 1 to 20 carbon atoms in which one or more -CH- groups are substituted with -O-, -S-, -NH-, -N(CH)-, -C(=O)-, -OC(=O)-, or -C(=O)O-; Q 1 and Q 2 each independently represents a hydrogen atom or a polymerizable group selected from the group consisting of groups represented by the following formulas Q-1 to Q-5, 1 and Q 2 represents a polymerizable group.

[0100]

[0101] In formula (I), the phenylene group is preferably a 1,4-phenylene group. When the phenylene group and trans-1,4-cyclohexylene group are referred to as "optionally having a substituent," the substituent is not particularly limited, and examples thereof include a substituent selected from the group consisting of an alkyl group, a cycloalkyl group, an alkoxy group, an alkyl ether group, an amide group, an amino group, a halogen atom, and a group formed by combining two or more of the above-mentioned substituents. In addition, examples of the substituent include the -C(=O)-X group described below. 3 -Sp 3 -Q 3 The phenylene group and the trans-1,4-cyclohexylene group may have 1 to 4 substituents. When the phenylene group and the trans-1,4-cyclohexylene group have two or more substituents, the two or more substituents may be the same or different.

[0102] The alkyl group may be either linear or branched. The alkyl group preferably has 1 to 30 carbon atoms, more preferably 1 to 10, and even more preferably 1 to 6. Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an isopentyl group, a neopentyl group, a 1,1-dimethylpropyl group, an n-hexyl group, an isohexyl group, a linear or branched heptyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, or a dodecyl group. The above description of the alkyl group also applies to an alkoxy group containing an alkyl group. Specific examples of the alkylene group include divalent groups obtained by removing any one hydrogen atom from each of the above alkyl group examples. Examples of halogen atoms include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.

[0103] The number of carbon atoms in the cycloalkyl group is preferably 3 to 20, more preferably 5 or more, and is preferably 10 or less, more preferably 8 or less, and even more preferably 6 or less. Examples of the cycloalkyl group include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, and a cyclooctyl group.

[0104] Substituents that the phenylene group and trans-1,4-cyclohexylene group may have include an alkyl group, an alkoxy group, and —C(═O)—X 3 -Sp 3 -Q 3 Preferred are substituents selected from the group consisting of: 3 is a single bond, -O-, -S-, or -N(Sp 4 -Q 4 ) - or Q 3 and Sp 3 The nitrogen atom forming a ring structure with Sp is shown. 3 and Sp 4each independently represents a linking group selected from the group consisting of a single bond, a linear or branched alkylene group having 1 to 20 carbon atoms, and a linear or branched alkylene group having 1 to 20 carbon atoms in which one or more -CH2- groups are replaced with -O-, -S-, -NH-, -N(CH3)-, -C(=O)-, -OC(=O)-, or -C(=O)O-.

[0105] Q 3 and Q 4 each independently represents a polymerizable group selected from the group consisting of a hydrogen atom, a cycloalkyl group, a cycloalkyl group in which one or more -CH2- groups are substituted with -O-, -S-, -NH-, -N(CH3)-, -C(=O)-, -OC(=O)-, or -C(=O)O-, or groups represented by formulae Q-1 to Q-5.

[0106] Specific examples of cycloalkyl groups in which one or more -CH2- groups are substituted with -O-, -S-, -NH-, -N(CH3)-, -C(=O)-, -OC(=O)-, or -C(=O)O- include a tetrahydrofuranyl group, a pyrrolidinyl group, an imidazolidinyl group, a pyrazolidinyl group, a piperidyl group, a piperazinyl group, and a morpholinyl group. The substitution position is not particularly limited. Of these, a tetrahydrofuranyl group is preferred, and a 2-tetrahydrofuranyl group is particularly preferred.

[0107] In formula (I), L is a single bond, —CHO—, —OCH 2- , -(CH2)2OC(=O)-, -C(=O)O(CH2)2-, -C(=O)O-, -OC(=O)-, -OC(=O)O-, -CH=CH-C(=O)O-, and -OC(=O)-CH=CH-. L is preferably -C(=O)O- or -OC(=O)-. The m-1 Ls may be the same or different.

[0108] Sp 1 and Sp 2each independently represents a linking group selected from the group consisting of a single bond, a linear or branched alkylene group having 1 to 20 carbon atoms, and a linear or branched alkylene group having 1 to 20 carbon atoms in which one or more -CH2- groups are replaced with -O-, -S-, -NH-, -N(CH3)-, -C(=O)-, -OC(=O)-, or -C(=O)O-. 1 and Sp 2 are preferably each independently a linear alkylene group having 1 to 10 carbon atoms bonded to both terminals with linking groups selected from the group consisting of -O-, -OC(=O)-, and -C(=O)O-, or a linking group formed by combining one or more groups selected from the group consisting of -OC(=O)-, -C(=O)O-, -O-, and linear alkylene groups having 1 to 10 carbon atoms, and are preferably linear alkylene groups having 1 to 10 carbon atoms bonded to both terminals with -O-.

[0109] Q 1 and Q 2 each independently represents a hydrogen atom or a polymerizable group selected from the group consisting of groups represented by the above formulas Q-1 to Q-5, 1 and Q 2 represents a polymerizable group. The polymerizable group is preferably an acryloyl group (formula Q-1) or a methacryloyl group (formula Q-2).

[0110] In formula (I), m represents an integer of 3 to 12. m is preferably an integer of 3 to 9, more preferably an integer of 3 to 7, and even more preferably an integer of 3 to 5.

[0111] The polymerizable compound represented by formula (I) preferably contains, as A, at least one phenylene group which may have a substituent and at least one trans-1,4-cyclohexylene group which may have a substituent. The polymerizable compound represented by formula (I) preferably contains, as A, 1 to 4 trans-1,4-cyclohexylene groups which may have a substituent, more preferably 1 to 3, and even more preferably 2 or 3. The polymerizable compound represented by formula (I) also preferably contains, as A, one or more phenylene groups which may have a substituent, more preferably 1 to 4, even more preferably 1 to 3, and particularly preferably 2 or 3.

[0112] In formula (I), when mc is the number obtained by dividing the number of trans-1,4-cyclohexylene groups represented by A by m, 0.1<mc<0.9 is preferred, 0.3<mc<0.8 is more preferred, and 0.5<mc<0.7 is even more preferred. It is also preferred that the liquid crystal composition contains a polymerizable compound represented by formula (I) where 0.1<mc<0.3, in addition to a polymerizable compound represented by formula (I) where 0.5<mc<0.7.

[0113] Specific examples of the polymerizable compound represented by formula (I) include the compounds described in paragraphs 0051 to 0058 of WO2016 / 047648, as well as compounds described in JP2013-112631A, JP2010-070543A, Japanese Patent No. 4725516, WO2015 / 115390, WO2015 / 147243, WO2016 / 035873, JP2015-163596A, and JP2016-053149A.

[0114] (Chiral Agent: Optically Active Compound) A chiral agent has the function of inducing a helical structure in a cholesteric liquid crystal phase. Chiral compounds can be selected according to the purpose, as the sense or pitch of the helix induced varies depending on the compound. The chiral agent is not particularly limited, and known compounds can be used. Examples of chiral agents include those described in Liquid Crystal Device Handbook (Chapter 3, Section 4-3, Chiral Agents for TN and STN, p. 199, edited by the 142nd Committee of the Japan Society for the Promotion of Science, 1989), JP-A Nos. 2003-287623, 2002-302487, 2002-080478, 2002-080851, 2010-181852, and 2014-034581.

[0115] Chiral agents generally contain an asymmetric carbon atom, but axially asymmetric or planarly asymmetric compounds that do not contain an asymmetric carbon atom can also be used as chiral agents. Examples of axially asymmetric or planarly asymmetric compounds include binaphthyl, helicene, paracyclophane, and derivatives thereof. The chiral agent may have a polymerizable group. When both the chiral agent and the liquid crystal compound have a polymerizable group, a polymer having a repeating unit derived from the polymerizable liquid crystal compound and a repeating unit derived from the chiral agent can be formed by polymerization of the polymerizable chiral agent and the polymerizable liquid crystal compound. In this embodiment, the polymerizable group of the polymerizable chiral agent is preferably the same type of group as the polymerizable group of the polymerizable liquid crystal compound. Therefore, the polymerizable group of the chiral agent is preferably an unsaturated polymerizable group, an epoxy group, or an aziridinyl group, more preferably an unsaturated polymerizable group, and particularly preferably an ethylenically unsaturated polymerizable group. The chiral agent may also be a liquid crystal compound.

[0116] As the chiral dopant, isosorbide derivatives, isomannide derivatives, binaphthyl derivatives, and the like can be preferably used. As the isosorbide derivative, a commercially available product such as LC756 manufactured by BASF may be used. The content of the chiral dopant in the liquid crystal composition is preferably 0.01 to 200 mol %, more preferably 1 to 30 mol %, relative to the amount of the polymerizable liquid crystal compound. The content of the chiral dopant in the liquid crystal composition refers to the concentration (% by mass) of the chiral dopant relative to the total solid content in the composition.

[0117] As described above, the reflective layer of the laminated glass of the present invention may be a cholesteric liquid crystal layer having two or more selective reflection center wavelengths. A cholesteric liquid crystal layer having two or more selective reflection center wavelengths can be achieved by changing the pitch of the helical structure in the thickness direction. A cholesteric liquid crystal layer whose helical structure pitch changes in the thickness direction can be produced by changing the amount of light irradiation in the thickness direction when forming a cholesteric liquid crystal layer using a chiral agent whose helical twisting power (HTP) changes when irradiated with light.

[0118] Examples of chiral agents whose HTP changes upon irradiation with light include those that undergo back-isomerization, dimerization, isomerization and dimerization, etc. When the chiral agent has a photoisomerizable group, the photoisomerizable group is preferably an isomerization site of a compound exhibiting photochromic properties, an azo group, an azoxy group, or a cinnamoyl group. Specific examples of the compound include compounds described in JP-A-2002-080478, JP-A-2002-080851, JP-A-2002-179668, JP-A-2002-179669, JP-A-2002-179670, JP-A-2002-179681, JP-A-2002-179682, JP-A-2002-338575, JP-A-2002-338668, JP-A-2003-313189, and JP-A-2003-313292.

[0119] (Polymerization Initiator) The liquid crystal composition preferably contains a polymerization initiator. In an embodiment in which the polymerization reaction is caused to proceed by ultraviolet irradiation, the polymerization initiator used is preferably a photopolymerization initiator capable of initiating the polymerization reaction by ultraviolet irradiation. Examples of the photopolymerization initiator include α-carbonyl compounds (described in U.S. Pat. Nos. 2,367,661 and 2,367,670), acyloin ethers (described in U.S. Pat. No. 2,448,828), α-hydrocarbon-substituted aromatic acyloin compounds (described in U.S. Pat. No. 2,722,512), polynuclear quinone compounds (described in U.S. Pat. Nos. 3,046,127 and 2,951,758), combinations of triarylimidazole dimers and p-aminophenyl ketones (described in U.S. Pat. No. 3,549,367), acridine and phenazine compounds (described in JP-A-60-105667 and U.S. Pat. No. 4,239,850), and acylphosphites. Benzene oxide compounds (JP-B No. 63-040799, JP-B No. 5-029234, JP-A No. 10-095788, JP-A No. 10-029997, JP-A No. 2001-233842, JP-A No. 2000-080068, JP-A No. 2006-342166, JP-A No. 2013-114249, JP-A No. 201 Examples of such compounds include those described in JP-A-2000-066385 and JP-A-2010-262028, JP-A-2014-500852, oxime compounds (described in JP-A-2000-066385 and JP-A-4454067), and oxadiazole compounds (described in U.S. Pat. No. 4,212,970). For example, the description in paragraphs 0500 to 0547 of JP-A-2012-208494 can also be taken into consideration.

[0120] As the polymerization initiator contained in the liquid crystal composition, it is also preferable to use an acylphosphine oxide compound or an oxime compound. As the acylphosphine oxide compound, for example, the commercially available product IRGACURE810 (compound name: bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide) manufactured by BASF Japan Ltd. can be used. As the oxime compound, commercially available products such as IRGACUREOXE01 (manufactured by BASF), IRGACUREOXE02 (manufactured by BASF), TR-PBG-304 (manufactured by Changzhou Strong Electronic New Materials Co., Ltd.), ADEKA ARCLES NCI-831, ADEKA ARCLES NCI-930 (manufactured by ADEKA), and ADEKA ARCLES NCI-831 (manufactured by ADEKA) can be used. Only one type of polymerization initiator may be used, or two or more types may be used in combination. The content of the photopolymerization initiator in the liquid crystal composition is preferably 0.1 to 20% by mass, more preferably 0.5 to 5% by mass, based on the content of the polymerizable liquid crystal compound.

[0121] (Crosslinking Agent) The liquid crystal composition may optionally contain a crosslinking agent in order to improve the film strength and durability after curing. As the crosslinking agent, one that is cured by ultraviolet light, heat, moisture, etc. can be suitably used. The crosslinking agent is not particularly limited and can be appropriately selected depending on the purpose. Examples of crosslinking agents include polyfunctional acrylate compounds such as trimethylolpropane tri(meth)acrylate and pentaerythritol tri(meth)acrylate; epoxy compounds such as glycidyl (meth)acrylate and ethylene glycol diglycidyl ether; aziridine compounds such as 2,2-bishydroxymethylbutanol-tris[3-(1-aziridinyl)propionate] and 4,4-bis(ethyleneiminocarbonylamino)diphenylmethane; isocyanate compounds such as hexamethylene diisocyanate and biuret isocyanate; polyoxazoline compounds having an oxazoline group in the side chain; and alkoxysilane compounds such as vinyltrimethoxysilane and N-(2-aminoethyl)3-aminopropyltrimethoxysilane. Furthermore, known catalysts can be used depending on the reactivity of the crosslinking agent, which can improve productivity in addition to improving film strength and durability. These may be used alone or in combination of two or more. The content of the crosslinking agent is preferably 3 to 20% by mass, more preferably 5 to 15% by mass, relative to the content of the polymerizable liquid crystal compound. By setting the content of the crosslinking agent to 3% by mass or more, the effect of improving the crosslinking density can be obtained, and by setting the content of the crosslinking agent to 20% by mass or less, a decrease in the stability of the cholesteric liquid crystal layer can be prevented. Note that "(meth)acrylate" is used to mean "either one or both of acrylate and methacrylate."

[0122] (Alignment Control Agent) An alignment control agent that contributes to stably or quickly forming a planar-aligned cholesteric liquid crystal layer may be added to the liquid crystal composition. Examples of the alignment control agent include fluorine (meth)acrylate polymers described in paragraphs

[0018] to

[0043] of JP-A No. 2007-272185, compounds represented by formulas (I) to (IV) described in paragraphs

[0031] to

[0034] of JP-A No. 2012-203237, and compounds described in JP-A No. 2013-113913. Note that one type of alignment control agent may be used alone, or two or more types may be used in combination.

[0123] Specific examples of compounds that can be used as alignment control agents include the following alignment control agent 1 and alignment control agent 2.

[0124]

[0125]

[0126] The amount of the alignment control agent added in the liquid crystal composition is preferably 0.01 to 10% by mass, more preferably 0.01 to 5% by mass, and even more preferably 0.02 to 1% by mass, based on the total mass of the polymerizable liquid crystal compound.

[0127] (Other Additives) The liquid crystal composition may further contain at least one selected from various additives such as a surfactant for adjusting the surface tension of the coating film and making the thickness uniform, and a polymerizable monomer, etc. Furthermore, if necessary, a polymerization inhibitor, an antioxidant, an ultraviolet absorber, a light stabilizer, a colorant, metal oxide fine particles, etc. may be further added to the liquid crystal composition within a range that does not deteriorate the optical performance.

[0128] The cholesteric liquid crystal layer can be formed by applying a liquid crystal composition prepared by dissolving a polymerizable liquid crystal compound and a polymerization initiator, and optionally a chiral agent, a surfactant, etc., in a solvent onto a transparent resin substrate, a retardation layer, an alignment layer, or a previously prepared cholesteric liquid crystal layer, etc., and drying the composition to obtain a coating film, which is then irradiated with actinic rays to polymerize the cholesteric liquid crystal composition, thereby forming a cholesteric liquid crystal layer with fixed cholesteric regularity. Note that a laminate film consisting of multiple cholesteric liquid crystal layers can be formed by repeatedly performing the above-mentioned production process for the cholesteric liquid crystal layer.

[0129] (Solvent) The solvent used for preparing the liquid crystal composition is not particularly limited and can be appropriately selected depending on the purpose, but an organic solvent is preferably used. The organic solvent is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include ketones, alkyl halides, amides, sulfoxides, heterocyclic compounds, hydrocarbons, esters, and ethers. These may be used alone or in combination of two or more. Among these, ketones are particularly preferred when considering the environmental impact.

[0130] (Coating, Alignment, Polymerization) The method for applying the liquid crystal composition to the transparent resin substrate, alignment layer, underlying cholesteric liquid crystal layer, etc. is not particularly limited and can be appropriately selected depending on the purpose. Examples of the coating method include wire bar coating, curtain coating, extrusion coating, direct gravure coating, reverse gravure coating, die coating, spin coating, dip coating, spray coating, and slide coating. Alternatively, the liquid crystal composition can be applied to a support and transferred onto the support. The applied liquid crystal composition is heated to align the liquid crystal molecules. The heating temperature is preferably 200°C or lower, more preferably 130°C or lower. This alignment treatment results in an optical thin film in which the polymerizable liquid crystal compound is twisted and aligned so that its helical axis is substantially perpendicular to the film surface.

[0131] The aligned liquid crystal compound can be further polymerized to harden the liquid crystal composition. The polymerization may be either thermal polymerization or photopolymerization using light irradiation, but photopolymerization is preferred. The light irradiation is preferably performed using ultraviolet light. The irradiation energy is 20 mJ / cm. 2 ~50 J / cm 2 is preferred, and 100 to 1,500 mJ / cm 2 is more preferable. In order to promote the photopolymerization reaction, light irradiation may be carried out under heated conditions or in a nitrogen atmosphere. The wavelength of the ultraviolet light to be irradiated is preferably 350 to 430 nm. From the viewpoint of stability, a higher polymerization reaction rate is preferable, preferably 70% or more, and more preferably 80% or more. The polymerization reaction rate can be determined by measuring the consumption rate of polymerizable functional groups using infrared absorption spectroscopy.

[0132] When the reflective layer is made of a dielectric layer and a metal layer, it is preferably formed by sandwiching the metal layer between the dielectric layers. Furthermore, since the phase of the reflective layer can be controlled by the refractive index and film thickness of the metal and dielectric layers, it is desirable to configure the reflective layer so that p-polarized light reflection at an incident angle of 65° is large.

[0133] The dielectric layer and the metal layer when the reflective layer is made up of a dielectric layer and a metal layer will be described below.

[0134] <Dielectric layer> The dielectric layer is formed by vapor phase deposition such as magnetron sputtering, and is made of ZnSnMgOx, ZnSnOx, ZnO, SnO 2 , TiO 2 , Si 3 N 4 , SiO 2 , MgF 2 The metal layer is preferably made of AlN or the like. When pure Ag is used for the metal layer, it is desirable that the dielectric layer function as an oxygen barrier layer to suppress oxidation of the metal layer. Furthermore, when a metal oxide film is formed by sputtering, the metal layer is oxidized when exposed to oxygen plasma, so it is desirable that the dielectric layer adjacent to the metal layer be a non-metal oxide film such as a nitride film. The dielectric layer may be an alternating layer of high refractive index layers and low refractive index layers with a thickness of 1 to 300 nm, and the phase can be controlled by adjusting the film thickness and refractive index, thereby controlling the transmittance and reflectance.

[0135] <Metal Layer> The lower the refractive index of the metal layer, the higher the p-polarized light reflectance at an incident angle of 65° can be. The refractive index at a wavelength of 550 nm is preferably 0.1 or less, more preferably 0.05 or less, and even more preferably 0.03 or less. In this respect, pure Ag is desirable for the metal layer. Pure silver is easily oxidized and has an unstable refractive index, so Ag alloys are sometimes used when forming a film by sputtering, but even in this case, it is desirable to keep the refractive index as low as possible.

[0136] <Transparent Resin Substrate> The transparent resin substrate is used as a substrate when forming, for example, a reflective layer, an adhesive layer, or a hard coat layer. The transparent resin substrate is preferably transparent in the visible light region.

[0137] There are no limitations on the material of the transparent resin substrate, and examples of the transparent resin substrate include plastic films such as polyesters such as polyethylene terephthalate (PET), polycarbonates, acrylic resins, epoxy resins, polyurethanes, polyamides, polyimides, polyolefins, cellulose derivatives, and silicones.

[0138] The thickness of the transparent resin substrate may be about 5.0 to 1000 μm, preferably 10 to 250 μm, and more preferably 15 to 90 μm.

[0139] (Method for forming a film from a transparent resin substrate) The transparent resin substrate may be formed into a film by any method, for example, a melt film-forming method or a solution film-forming method.

[0140] <Melt film-forming method, smoothing> When a transparent resin substrate is formed into a film by a melt film-forming method, it is preferable to include a melting step of melting the resin in an extruder, a step of extruding the molten resin into a sheet form from a die, and a step of forming into a film. Depending on the material of the resin, a filtering step of the molten resin may be provided after the melting step, or the molten resin may be cooled when extruded into a sheet form. Below, specific melt film-forming methods will be described, but the present invention is not limited thereto.

[0141] [Method for forming a transparent resin substrate] The method for producing the transparent resin substrate includes a melting step in which a resin is melted in an extruder, a filtration step in which the molten resin is filtered through a filtration device equipped with a filter, a film forming step in which the filtered resin is extruded into a sheet form through a die and brought into close contact with a cooling drum to be cooled and solidified to form an unstretched transparent resin substrate, and a stretching step in which the unstretched transparent resin substrate is stretched uniaxially or biaxially. This configuration allows the transparent resin substrate to be produced. If the pore size of the filter used in the filtration step of the molten resin is 1 μm or less, foreign matter can be sufficiently removed. As a result, the surface roughness in the film width direction of the obtained transparent resin substrate can be controlled. Specifically, the method for forming a transparent resin substrate includes the following steps.

[0142] <Melting Step> The method for producing the transparent resin substrate includes a melting step in which the resin is melted in an extruder. The resin, or a mixture of the resin and additives, is preferably dried to a moisture content of 200 ppm or less, and then introduced into a single-screw (single-screw) or twin-screw extruder and melted. At this time, melting in nitrogen or vacuum is also preferred to suppress decomposition of the resin. Detailed conditions can be implemented according to <0051> to <0052> of Japanese Patent No. 4962661 (<0085> to <0086> of US 2013 / 0100378), and the contents of these publications are incorporated herein by reference. The extruder is preferably a single-screw kneading extruder. Furthermore, it is also preferable to use a gear pump to increase the delivery accuracy of the molten resin (melt).

[0143] The method for producing a transparent resin substrate includes a filtration step of filtering a molten resin through a filtration device equipped with a filter, and the pore size of the filter used in the filtration step is preferably 1 μm or less. Only one set of filtration devices having filters with such pore sizes may be installed in the filtration step, or two or more sets of filtration devices may be installed.

[0144] <Film Forming Step> The method for producing the transparent resin substrate includes a film forming step in which the filtered resin is extruded into a sheet form through a die and brought into close contact with a cooling drum to be cooled and solidified to form an unstretched transparent resin substrate.

[0145] When the melted (and kneaded) and filtered resin (melt containing the resin) is extruded into a sheet form through a die, it may be extruded as a single layer or as a multilayer. When extruding as a multilayer, for example, a layer containing an ultraviolet absorber and a layer not containing an ultraviolet absorber may be laminated, and a three-layer structure in which a layer containing an ultraviolet absorber is the inner layer is more preferable in terms of suppressing deterioration of the polarizer due to ultraviolet rays and suppressing bleed-out of the ultraviolet absorber. When a transparent resin substrate is produced by extruding a multilayer, the thickness of the inner layer of the obtained transparent resin substrate relative to the thickness of all layers is preferably 50 to 99%, more preferably 60 to 99%, and even more preferably 70 to 99%. Such lamination can be performed using a feed block die or a multi-manifold die.

[0146] According to <0059> of JP2009-269301A, it is preferable to extrude a resin (a melt containing a resin) extruded into a sheet form from a die onto a cooling drum (a casting drum), cool and solidify it, and obtain an unstretched transparent resin substrate (raw sheet).

[0147] In the method for producing the transparent resin substrate, the temperature of the resin extruded from the die is preferably 280 to 320°C, more preferably 285 to 310°C. It is preferable that the temperature of the resin extruded from the die in the melting step is 280°C or higher, since this reduces the amount of unmelted raw resin and suppresses the generation of foreign matter. It is preferable that the temperature of the resin extruded from the die in the melting step is 320°C or lower, since this reduces the decomposition of the resin and suppresses the generation of foreign matter. The temperature of the resin extruded from the die can be measured non-contact with the surface of the resin using a radiation thermometer (manufactured by Hayashi Denko, model number: RT61-2, emissivity 0.95).

[0148] In the method for producing the transparent resin substrate, it is preferable to use an electrostatically applied electrode when the resin is brought into close contact with the cooling drum in the film forming step, which allows the resin to be tightly attached to the cooling drum without roughening the film surface.

[0149] In the method for producing the transparent resin substrate, the temperature of the resin when it is brought into close contact with the cooling drum (at the point where the molten resin extruded from the die first comes into contact with the cooling drum) is preferably 280°C or higher. This increases the electrical conductivity of the resin, allowing it to be tightly adhered to the cooling drum by applying static electricity, and suppressing roughness of the film surface. The temperature of the resin when it is brought into close contact with the cooling drum can be measured by contactless measurement of the resin surface using a radiation thermometer (manufactured by Hayashi Denko, model number: RT61-2, emissivity 0.95).

[0150] The method for producing the transparent resin substrate includes a stretching step of uniaxially or biaxially stretching the unstretched transparent resin substrate. In the longitudinal stretching step (stretching in the same direction as the film transport direction), the transparent resin substrate is preheated and then stretched in the transport direction with a group of rollers having different peripheral speeds (i.e., different transport speeds) while the transparent resin substrate is still heated.

[0151] The preheating temperature in the longitudinal stretching step is preferably Tg-40°C or higher and Tg+60°C or lower, more preferably Tg-20°C or higher and Tg+40°C or lower, and even more preferably Tg or higher and Tg+30°C or lower, relative to the glass transition temperature (Tg) of the transparent resin substrate. The stretching temperature in the longitudinal stretching step is preferably Tg or higher and Tg+60°C or lower, more preferably Tg+2°C or higher and Tg+40°C or lower, and even more preferably Tg+5°C or higher and Tg+30°C or lower. The stretching ratio in the longitudinal direction is preferably 1.0 times or higher and 2.5 times or lower, and more preferably 1.1 times or higher and 2 times or lower.

[0152] In addition to or instead of the longitudinal stretching step, the transparent resin substrate is stretched transversely in the width direction by a transverse stretching step (a step of stretching in a direction perpendicular to the film conveying direction). In the transverse stretching step, for example, a tenter can be suitably used, and the transparent resin substrate is stretched transversely by this tenter while holding both widthwise ends with clips. This transverse stretching can increase the tensile modulus of the transparent resin substrate in the optical film.

[0153] The transverse stretching is preferably carried out using a tenter, and the stretching temperature is preferably from Tg to Tg + 60°C, more preferably from Tg + 2°C to Tg + 40°C, and even more preferably from Tg + 4°C to Tg + 30°C, relative to the glass transition temperature (Tg) of the transparent resin substrate. The stretching ratio is preferably from 1.0 to 5.0 times, and more preferably from 1.1 to 4.0 times. It is also preferable to relax the transparent resin substrate in either the longitudinal direction or the transverse direction, or both, after the transverse stretching.

[0154] Furthermore, it is preferable that the thickness variation depending on the location in both the width direction and the length direction be 10% or less, more preferably 8% or less, even more preferably 6% or less, particularly preferably 4% or less, and most preferably 2% or less.

[0155] The thickness variation can be calculated as follows.

[0156] A 10 m (meter) sample of the stretched transparent resin substrate is taken, and 20% of each end of the film width direction is removed. 50 samples are taken at equal intervals in both the width direction and the length direction from the center of the film, and the thickness is measured.

[0157] Average thickness in the width direction Th TD-av , maximum value Th TD-max , minimum value Th TD-min , (Th TD-max -Th TD-min ) ÷ Th TD-av ×100[%] is the thickness variation in the width direction.

[0158] In addition, the average thickness in the longitudinal direction Th MD-av , maximum value Th MD-max , minimum value Th MD-min, (Th MD-max -Th MD-min ) ÷ Th MD-av ×100[%] is the thickness variation in the longitudinal direction.

[0159] The stretching step can improve the thickness accuracy of the transparent resin substrate.

[0160] The stretched transparent resin substrate can be wound into a roll in a winding process. At this time, the winding tension of the transparent resin substrate is 0.02 kg / mm 2 It is preferable to do the following:

[0161] Regarding other detailed conditions, the contents described in <0134> to <0148> of JP2015-224267A for the melt film-forming process and the contents described in JP2007-137028A for the stretching process can be incorporated into this specification in accordance with the present invention.

[0162] <Solution Casting Method, Smoothing> When a transparent resin substrate is formed into a film by a solution casting method, the method preferably includes the steps of casting a dope solution onto a casting band to form a cast film, drying the cast film, and stretching the cast film. Specifically, the film is preferably formed by the method described in Japanese Patent No. 4,889,335. In the present invention, the following method is preferably employed. For example, JP-A-11-123732 discloses a method of drying the cast film slowly by setting the drying rate of the cast film to 300% by mass / min (=5% by mass / s) or less in terms of the solvent content on a dry basis. Also, JP-A-2003-276037 discloses a method of co-casting a multilayered cast film having a core layer (an intermediate layer) and skin layers (outer layers) on both surfaces thereof, in which the viscosity of the dope forming the core layer is increased to ensure the strength of the cast film and the viscosity of the dope forming the outer layers is reduced. Further, there are also preferred methods such as a method in which the casting film is rapidly dried to form a film on the surface of the casting film, and the surface condition is smoothed by the leveling effect of the formed film, and a method in which the casting film is stretched.

[0163] The transparent resin substrate may be thermally shrunk. This is particularly advantageous when the film is adapted to conform to a curved glass surface, as the thermal shrinkage of the transparent resin substrate causes the film to shrink and wrinkles to be suppressed. It is believed that when a flat film is sandwiched between curved glass, wrinkles caused by excess film can be eliminated by shrinkage of the film containing the transparent resin substrate. Generally, transparent resin substrates are stretched during production, and stress resulting from the stretching exists as residual stress. Therefore, this residual stress can be utilized to cause thermal shrinkage by heating during conforming to the curved surface. It is believed that this thermal shrinkage can eliminate wrinkles that occur when the film is adapted to conform to the curved glass surface. Furthermore, wrinkles tend to occur in areas of the glass near the periphery where the curvature is greater, but are less likely to occur in areas where the curvature is smaller. In contrast, a film using a thermally shrinkable transparent resin substrate effectively suppresses wrinkles in areas of the glass where the curvature is greater. The mechanism of action is thought to be that in areas of greater curvature of the glass, the film has the freedom to expand in the thickness direction, resulting in film shrinkage in the surface direction, while in areas of less curvature of the glass, the film has less freedom to expand in the thickness direction, resulting in almost no film shrinkage in the surface direction. The temperature at which the transparent resin substrate thermally shrinks varies depending on the material from which the transparent resin substrate is formed, but shrinkage is preferably in the range of 80 to 200°C, and more preferably in the range of 100 to 140°C, which is the heating temperature using a heat gun in a typical curved surface conforming process. Heating to shrink the transparent resin substrate may be applied to the entire curved glass, or may be applied locally to areas with high curvature that are prone to wrinkling. The amount of shrinkage of the transparent resin substrate required to suppress film wrinkling varies depending on the curvature and dimensions of the glass, etc. Under heating conditions using a heat gun or the like in the curved surface conforming process, the transparent resin substrate preferably has a heat shrinkage rate of 0.01 to 5.0%, more preferably 0.05 to 3.0%, and even more preferably 0.2 to 2.0%, in both the direction in which the heat shrinkage rate is greatest and the direction perpendicular to that direction, respectively. When the heat shrinkage rate is 0.01% or more, wrinkles are less likely to occur when the substrate conforms to a curved surface. Furthermore, when the heat shrinkage rate is 5.0% or less, bubbles are less likely to occur when the substrate conforms to a curved surface.The heat shrinkage rate can be appropriately adjusted by adjusting the stretching conditions when producing the transparent resin substrate.

[0164] <Measurement of Heat Shrinkage Rate> Two reference lines are marked in advance in the width direction at a distance of 100 mm on a film sample piece cut to a width of 30 mm and a length of 120 mm. The sample piece is left to stand in a heating oven at 140°C for 45 minutes under no tension, and then cooled to room temperature, and the distance between the two reference lines is measured. The measured distance after treatment is designated as A [mm]. The value [%] calculated from the distance of 100 mm before treatment and the distance A mm after treatment using the formula "100 x (100 - A) / 100" is the heat shrinkage rate of the sample piece.

[0165] <Adhesive Layer> The laminated glass of the present invention may have an adhesive layer for bonding the glass and the transparent resin substrate or the reflective layer. The adhesive layer makes it possible to integrate the glass and the transparent resin substrate or the reflective layer. The adhesive layer is not particularly limited in material as long as it has transparency that ensures visibility of the display content when attached to glass and can bond the transparent resin substrate or the reflective layer to the glass, and may be made of a resin or an elastomer (including oil-extended rubber). In addition, the adhesive layer may be a layer that plasticizes and develops adhesiveness due to the heat during processing of the laminated glass (heat seal layer), or a layer that has adhesiveness at room temperature and is attached after processing of the laminated glass (adhesive layer).

[0166] <Heat Seal Layer> The laminated glass of the present invention may have a heat seal layer as an adhesive layer. The heat seal layer is plasticized by heat to exhibit adhesiveness, and serves to physically bond the transparent resin substrate or the reflective layer to the glass substrate.

[0167] The heat seal layer contains a thermoplastic resin, preferably one having good affinity and adhesiveness with the glass substrate, and preferably a resin selected from the group consisting of polyvinyl acetal resins typified by polyvinyl butyral (PVB) resin, ethylene-vinyl acetate copolymers, and chlorine-containing resins, more preferably polyvinyl butyral or ethylene-vinyl acetate copolymers.

[0168] Polyvinyl butyral can be obtained by acetalizing polyvinyl alcohol with butyraldehyde. The degree of acetalization of polyvinyl butyral is not particularly limited, but is preferably 40% or more, more preferably 60% or more. The upper limit is not particularly limited, but is preferably 85% or less, more preferably 75% or less. Polyvinyl alcohol used in the synthesis of polyvinyl butyral is usually obtained by saponifying polyvinyl acetate, and polyvinyl alcohol with a saponification degree of 80 to 99.8 mol% is generally used. The degree of polymerization of the polyvinyl alcohol is preferably 200 to 3000.

[0169] When the heat seal layer is provided adjacent to the reflective layer, the retardation layer, or the polarization conversion layer, it preferably contains a polymerizable compound for chemically bonding with the above-mentioned layer. The polymerizable compound is preferably one that can chemically bond with the polymerizable liquid crystal compound contained in the reflective layer, the retardation layer, or the polarization conversion layer, and for example, when the polymerizable liquid crystal compound has an ethylenically unsaturated polymerizable group, it is preferable that the polymerizable compound also has an ethylenically unsaturated polymerizable group.

[0170] Examples of the ethylenically unsaturated polymerizable group-containing compound include the following. However, the present invention is not limited to the following exemplified compounds. For example, polyethylene glycol 200 di(meth)acrylate, polyethylene glycol 300 di(meth)acrylate, polyethylene glycol 400 di(meth)acrylate, polyethylene glycol 600 di(meth)acrylate, triethylene glycol di(meth)acrylate, epichlorohydrin-modified ethylene glycol di(meth)acrylate (commercially available products include Denacol DA-811 manufactured by Nagase & Co., Ltd.), polypropylene glycol 200 di(meth)acrylate, polypropylene glycol 400 di(meth)acrylate, polypropylene glycol 700 di(meth)acrylate, ethylene oxide (EO), propylene oxide (PO),propylene oxide) block polyether di(meth)acrylate (commercially available products, such as the Blemmer PET series manufactured by Nippon Oil & Fats Co., Ltd.), dipropylene glycol di(meth)acrylate, bisphenol A EO addition type di(meth)acrylate (commercially available products, such as M-210 manufactured by Toagosei Co., Ltd. and NK Ester A-BPE-20 manufactured by Shin-Nakamura Chemical Co., Ltd.), hydrogenated bisphenol A EO addition type di(meth)acrylate (NK Ester A-HPE-4 manufactured by Shin-Nakamura Chemical Co., Ltd.), bisphenol A PO addition type di(meth)acrylate (commercially available products, such as Light Acrylate BP-4PA manufactured by Kyoeisha Chemical Co., Ltd.), bisphenol A epichlorohydrin addition type di(meth)acrylate (commercially available products, such as Ebecryl 150 manufactured by Daicel UCB Co., Ltd.), bisphenol A EO·PO addition type di(meth)acrylate (commercially available products include BP-023-PE manufactured by Toho Chemical Industry Co., Ltd.), bisphenol F Examples of bifunctional (meth)acrylate compounds include EO-added di(meth)acrylate (commercially available products include Aronix M-208 manufactured by Toagosei Co., Ltd.), 1,6-hexanediol di(meth)acrylate and epichlorohydrin-modified products thereof, neopentyl glycol di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate and caprolactone-modified products thereof, 1,4-butanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, trimethylolpropane di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, pentaerythritol di(meth)acrylate monostearate, trimethylolpropane acrylic acid benzoate, and EO-modified isocyanuric acid di(meth)acrylate (commercially available products include Aronix M-215 manufactured by Toagosei Co., Ltd.);

[0171] Further, trifunctional (meth)acrylate compounds such as trimethylolpropane tri(meth)acrylate (commercially available products include TPMTA manufactured by Nippon Kayaku Co., Ltd.) and its EO, PO, or epichlorohydrin-modified products, pentaerythritol tri(meth)acrylate, glycerol tri(meth)acrylate and its EO, PO, or epichlorohydrin-modified products, isocyanuric acid EO-modified tri(meth)acrylate (commercially available products include Aronix M-315 manufactured by Toagosei Co., Ltd.), tris(meth)acryloyloxyethyl phosphate, hydrogen phthalate-(2,2,2-tri-(meth)acryloyloxymethyl)ethyl, glycerol tri(meth)acrylate and its EO, PO, or epichlorohydrin-modified products; Examples of the ethylenically unsaturated polymerizable group-containing compounds include tetrafunctional (meth)acrylate compounds such as dipentaerythritol penta(meth)acrylate and its EO, PO, epichlorohydrin-modified products, and ditrimethylolpropane tetra(meth)acrylate; pentafunctional (meth)acrylate compounds such as dipentaerythritol penta(meth)acrylate and its EO, PO, epichlorohydrin-, fatty acid-, or alkyl-modified products; and hexafunctional (meth)acrylate compounds such as dipentaerythritol hexa(meth)acrylate and its EO, PO, epichlorohydrin-, fatty acid-, or alkyl-modified products, and sorbitol hexa(meth)acrylate and its EO, PO, epichlorohydrin-, fatty acid-, or alkyl-modified products. Two or more ethylenically unsaturated polymerizable group-containing compounds may be used in combination. In this case, a mixture of dipentaerythritol pentaacrylate and dipentaerythritol hexaacrylate, "DPHA" (manufactured by Nippon Kayaku Co., Ltd.), or the like can be preferably used.

[0172] Also preferred as the ethylenically unsaturated polymerizable group-containing compound are polyester(meth)acrylates and epoxy(meth)acrylates having a weight-average molecular weight of 200 or more and less than 1,000. Commercially available polyester(meth)acrylates include the Beamset 700 series (trade name) manufactured by Arakawa Chemical Industries, Ltd., such as Beamset 700 (hexafunctional), Beamset 710 (tetrafunctional), and Beamset 720 (trifunctional). Epoxy(meth)acrylates include the SP series (trade name) manufactured by Showa Polymer Co., Ltd., such as SP-1506, 500, SP-1507, and 480, and the VR series (trade name) VR-77, and Shin-Nakamura Chemical Co., Ltd., such as EA-1010 / ECA, EA-11020, EA-1025, and EA-6310 / ECA.

[0173] The I / O ratio (ratio of inorganic value (I value) to organic value (O value)) of the ethylenically unsaturated polymerizable group-containing compound is preferably 0.40 or more, more preferably 0.60 or more, and even more preferably 1.2 or more, from the viewpoint of adhesion to a glass substrate. There is no particular upper limit to the I / O ratio, but from the viewpoint of compatibility with a thermoplastic resin, it is preferably less than 3.0.

[0174] The I / O ratio is calculated using the calculation method in the organic conceptual diagram. The organic conceptual diagram was proposed by Fujita et al. and is an effective method for predicting various physicochemical properties from the chemical structure of an organic compound (see Koda Yoshio, Organic Conceptual Diagram - Fundamentals and Applications, Sankyo Publishing (1984)). Since the polarity of an organic compound depends on the number of carbon atoms and substituents, the inorganic value and organic value of other substituents are determined based on the organic value of the methylene group being 20 and the inorganic value of the hydroxyl group being 100, and the inorganic value and organic value of the organic compound are then calculated. Organic compounds with a high inorganic value have high polarity, and organic compounds with a high organic value have low polarity.

[0175] Specific methods for calculating the I value, O value, and I / O ratio have been published as an organic conceptual diagram calculation sheet for Excel by Homma et al., co-authors of "New Edition Organic Conceptual Diagram: Fundamentals and Applications" (http: / / www.ecosci.jp / sheet / orgs_help.html), and these calculations can be performed using this.

[0176] The content of the polymerizable compound in the heat seal layer is preferably 5 to 80% by mass, more preferably 10 to 60% by mass, and even more preferably 15 to 50% by mass, based on the total mass of the heat seal layer. By setting the content of the polymerizable compound in the heat seal layer within the above range, it is possible to achieve both adhesion to the glass substrate and adhesion to the reflective layer, retardation layer, or polarization conversion layer.

[0177] (i) Polymerization Initiator The photopolymerization initiator may be any one that can generate radicals as active species upon irradiation with light, and known photopolymerization initiators can be used without any limitations. Specific examples include diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, benzyl dimethyl ketal, 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-2-morpholino(4-thiomethylphenyl)propan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, 2-hydroxy-2-methyl-1-[4-(1-methyl) acetophenones such as 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one; oxime esters such as 1,2-octanedione, 1-[4-(phenylthio)-, 2-(O-benzoyloxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime); benzoyl benzoins such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether; benzophenone, methyl ortho-benzoylbenzoate, 4-phenylbenzophenone, 4-benzoyl-4'-methyl-diphenyl sulfide, 3,3',4,4'-tetra(t-butylperoxycarbonyl)benzophenone, 2,4,6-trimethylbenzophenone, 4-benzoyl-N,N-dimethyl-N-[2-(1-oxo-2 benzophenones such as (4-benzoylbenzyl)trimethylammonium bromide and (4-benzoylbenzyl)trimethylammonium chloride; thioxanthones such as 2-isopropylthioxanthone, 4-isopropylthioxanthone, 2,4-diethylthioxanthone, 2,4-dichlorothioxanthone, 1-chloro-4-propoxythioxanthone, and 2-(3-dimethylamino-2-hydroxy)-3,4-dimethyl-9H-thioxanthone-9-one mesochloride;and acylphosphine oxides such as 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide, and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide. Furthermore, as a coagent for the polymerization initiator, triethanolamine, triisopropanolamine, 4,4'-dimethylaminobenzophenone (Michler's ketone), 4,4'-diethylaminobenzophenone, 2-dimethylaminoethylbenzoic acid, ethyl 4-dimethylaminobenzoate, (n-butoxy)ethyl 4-dimethylaminobenzoate, isoamyl 4-dimethylaminobenzoate, 2-ethylhexyl 4-dimethylaminobenzoate, 2,4-diethylthioxanthone, 2,4-diisopropylthioxanthone, and the like may be used in combination. The above polymerization initiators and auxiliaries can be synthesized by known methods and are also available as commercial products. Preferred examples of commercially available radical photopolymerization initiators include Irgacure (127, 651, 184, 819, 907, 1870 (CGI-403 / Irg184=7 / 3 mixed initiator, 500, 369, 1173, 2959, 4265, 4263, etc.), OXE01) manufactured by BASF, KAYACURE (DETX-S, BP-100, BDMK, CTX, BMS, 2-EAQ, ABQ, CPTX, EPD, ITX, QTX, BTC, MCA, etc.) manufactured by Nippon Kayaku, and Esacure (KIP100F, KB1, EB3, BP, X33, KT046, KT37, KIP150, TZT) manufactured by Sartomer;

[0178] The content of the radical photopolymerization initiator contained in the heat-seal layer-forming composition is not particularly limited, and may be appropriately adjusted within a range in which the polymerization reaction of the radical polymerizable compound proceeds smoothly. The content of the radical photopolymerization initiator contained in the heat-seal layer-forming curable composition is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 1 to 10 parts by mass, relative to 100 parts by mass of the polymerizable compound.

[0179] The heat seal layer may contain inorganic particles. By including inorganic particles in the heat seal layer, unevenness is formed on the surface of the heat seal layer, reducing friction between the heat seal layer and the glass substrate, which is preferable as it is easy to handle during processing of laminated glass. As the inorganic particles contained in the heat seal layer, inorganic oxide particles are preferred, silica (silicon dioxide) particles, aluminum oxide particles, titanium dioxide particles, or zirconium oxide particles are more preferred, and silica particles are even more preferred.

[0180] The inorganic particles preferably consist of primary particles, with secondary particles formed by aggregation of the primary particles. The average primary particle size of the inorganic particles is not particularly limited, but is preferably 5 to 50 nm, more preferably 5 to 15 nm. The average secondary particle size of the inorganic particles is not particularly limited, but is preferably 100 to 500 nm.

[0181] The content of the inorganic particles in the heat seal layer is not particularly limited, but is preferably 1% by mass or more, more preferably 9% by mass or more, relative to the total mass of the heat seal layer. The upper limit is not particularly limited, but is preferably 40% by mass or less, more preferably 30% by mass or less.

[0182] The average primary particle diameter of inorganic particles is measured by observation with a transmission electron microscope. Specifically, the diameter of the circle circumscribing the primary particles is determined for 50 randomly selected primary particles, and the arithmetic mean is taken as the average primary particle diameter. The magnification of the transmission electron microscope is set to any magnification between 500,000 and 5,000,000 that allows the primary particle diameter to be determined. The average secondary particle diameter is a value measured by performing spherical fitting (refractive index 1.46) using a laser diffraction / scattering particle size distribution analyzer. For example, a MicroTrac MT3000 manufactured by Microtrac-Bell Corporation can be used as the measuring device.

[0183] The heat seal layer may contain a leveling agent. By including a leveling agent in the heat seal layer, the surface of the heat seal layer is smoothed, thereby improving visibility when integrated with a glass substrate. As the leveling agent, known leveling agents can be used, for example, surfactants, and among these, fluorine-based surfactants or silicone-based surfactants are preferred. The fluorine content in the fluorine-based surfactant is preferably 3 to 40% by mass, more preferably 5 to 30% by mass, and even more preferably 7 to 25% by mass. Fluorine-based surfactants with a fluorine content within this range are effective in terms of uniformity of the thickness of the coating film and liquid saving.

[0184] The content of the leveling agent in the heat seal layer is not particularly limited, but is preferably 0.005 to 0.5% by mass, more preferably 0.01 to 0.1% by mass, based on the total mass of the heat seal layer.

[0185] The water contact angle of the surface of the heat seal layer opposite the reflective layer or polarization conversion layer is not particularly limited, but is preferably 100° or less, more preferably 90° or less, and even more preferably 70° or less, in terms of better adhesion to the glass substrate. The lower limit is not particularly limited, but is often 10° or more, and more often 30° or more. The water contact angle is measured as follows. First, at three different locations on the heat seal layer surface of the film, a contact angle meter CA-X (manufactured by Kyowa Interface Science Co., Ltd.) is used to create 1.0 mm diameter droplets using pure water at the tip of a needle under an environment of 20°C and 65% RH, and these droplets are brought into contact with the surface of the heat seal layer to form droplets. 25 seconds after the heat seal layer surface comes into contact with the pure water, the angle formed by the tangent to the pure water surface and the heat seal layer surface at the point where the heat seal layer surface and the pure water come into contact is measured, and the average of these angles is taken as the water contact angle of the heat seal layer.

[0186] From the viewpoint of coatability, the composition for forming a heat seal layer preferably contains a solvent. The type of solvent is not particularly limited, and examples thereof include water and organic solvents, with organic solvents being preferred. Examples of organic solvents include ketones, alkyl halides, amides, sulfoxides, heterocyclic compounds, hydrocarbons, esters, and ethers.

[0187] The method for applying the composition for forming a heat seal layer is not particularly limited, and examples thereof include wire bar coating, curtain coating, extrusion coating, direct gravure coating, reverse gravure coating, die coating, spin coating, dip coating, spray coating, and slide coating.

[0188] The coating film obtained by coating may be subjected to a drying treatment, if necessary. Examples of the drying treatment include a heat treatment. The heating temperature in the heat treatment is not particularly limited, but is preferably 50 to 150°C, and more preferably 60 to 140°C. The heating time is not particularly limited, but is preferably 0.5 to 20 minutes, and more preferably 0.5 to 10 minutes.

[0189] The surface of the formed heat seal layer (the surface opposite to the transparent resin substrate, reflective layer, or polarization conversion layer) may be subjected to a surface treatment as needed. For example, in order to reduce the water contact angle of the surface of the heat seal layer, the surface of the heat seal layer may be subjected to a hydrophilization treatment. Examples of hydrophilization treatments include plasma treatment, ultraviolet irradiation treatment, corona treatment, and electron beam irradiation treatment, with corona treatment being preferred. The conditions for the hydrophilization treatment are appropriately selected depending on the type of treatment to be performed, and are preferably adjusted so that the water contact angle of the surface of the heat seal layer falls within the range described above.

[0190] The average thickness of the heat seal layer is preferably 0.2 μm or more, more preferably 0.4 μm or more, and even more preferably 0.8 μm or more, from the viewpoint of adhesion to the glass substrate, transparent resin substrate, reflective layer, or polarization conversion layer. The upper limit is not particularly limited, but from the viewpoint of thinning, it is preferably 20 μm or less, more preferably 10 μm or less. The average thickness is measured by cutting the heat seal layer with a microtome to cut out a cross section, observing the cross section with an SEM (Scanning Electron Microscope), measuring the thickness at three different positions on the heat seal layer, and calculating the average (arithmetic mean) of the measured values ​​to obtain the average thickness.

[0191] The heat-seal layer may have a single layer structure or a multi-layer structure of two or more layers. When the heat-seal layer has a multi-layer structure, the average total thickness of the heat-seal layer is preferably within the above range. That is, when the heat-seal layer is composed of two layers, heat-seal layer 1 and heat-seal layer 2, the average total thickness (average thickness) of heat-seal layer 1 and heat-seal layer 2 is preferably 0.4 μm or more.

[0192] <Adhesive Layer> The laminated glass of the present invention may have an adhesive layer as an adhesive layer. The adhesive layer has adhesiveness at room temperature and is a layer for adhering the glass to the transparent resin substrate or the reflective layer. The material of the adhesive layer is not particularly limited, and may be made of a resin or an elastomer (including oil-extended rubber).

[0193] Resins used in the adhesive layer include polyolefin resins such as 1,2-polybutadiene resin, ethylene-vinyl acetate copolymer (abbreviated as "EVA", usually containing 3% by mass or more of vinyl acetate constituent units), and polyethylene, polyvinyl chloride resin, polystyrene resin, vinyl ester resin (excluding EVA), saturated polyester resin, polyamide resin, fluororesin (polyvinylidene fluoride, etc.), polycarbonate resin, polyacetal resin, urethane resin, epoxy resin, (meth)acrylate resin (also referred to as (meth)acrylic resin, meaning (meth)acrylic acid ester resin, etc.), unsaturated polyester resin, silicone resin, and modified resins of these resins. Examples of urethane resins include urethane-modified polyester resin and urethane resin.

[0194] Examples of the elastomer include block (co)polymers of conjugated dienes, acrylic block (co)polymers, styrene block (co)polymers, block copolymers of aromatic vinyl compounds and conjugated dienes, hydrogenated products of block (co)polymers of conjugated dienes, hydrogenated products of block copolymers of aromatic vinyl compounds and conjugated dienes, ethylene-α-olefin copolymers, polar group-modified olefin copolymers, elastomers composed of polar group-modified olefin copolymers and metal ions and / or metal compounds, nitrile rubbers such as acrylonitrile-butadiene rubbers, butyl rubber, acrylic rubbers, thermoplastic elastomers such as thermoplastic polyolefin elastomers (TPO), thermoplastic polyurethane elastomers (TPU), thermoplastic polyester elastomers (TPEE), thermoplastic polyamide elastomers (TPAE), diene elastomers (1,2-polybutadiene, etc.), silicone elastomers, and fluorine-based elastomers.

[0195] The weight average molecular weight of the resin or elastomer is preferably 10,000 to 1,000,000, more preferably 50,000 to 500,000, from the viewpoint of the balance between solubility in a solvent and storage modulus.

[0196] When forming an adhesive layer, these resins or elastomers can be composed solely of polymers, or can also be composed of additives such as softeners, plasticizers, lubricants, crosslinking agents, crosslinking aids, photosensitizers, antioxidants, antiaging agents, heat stabilizers, flame retardants, antibacterial agents, mildew inhibitors, weather resistance agents, UV absorbers, tackifiers, nucleating agents, pigments, dyes, organic fillers, inorganic fillers, silane coupling agents, and titanium coupling agents, or compositions containing polymerizable group-containing compounds or other polymers. That is, the impact absorbing layer may be composed of a resin composition or an elastomer composition.

[0197] The adhesive layer may be made of a commercially available adhesive, such as SK Dyne 2057, SK Dyne 2094, SK Dyne 2147, SK Dyne 1811L, SK Dyne 1478, SK Dyne 1442, SK Dyne 1435, and SK Dyne 1415 (all manufactured by Soken Chemical & Engineering Co., Ltd.), NCF-N632, NCF-D692, NCF-F619, MO-T015, MO-5115XV (all manufactured by Lintec Corporation), TD06, and MK64. , TI14, ME57, TX48, MJ63, MG70, MF58 (all manufactured by Tomoegawa Paper Co., Ltd.), Panaclean PD-S1, Panaclean PD-R5 (all manufactured by Panac Corporation), MHM-FWD, MHM-FWV, MHM-UVC, MHM-SI (manufactured by Nichiei Shinka Co., Ltd.), Orivine EG-655, and Orivine BPS5896 (all manufactured by Toyo Ink Co., Ltd.) (all trade names) can be suitably used.

[0198] The thickness of the adhesive layer is preferably 100 μm or less, more preferably 50 μm or less, even more preferably 30 μm or less, particularly preferably more than 4 μm to 30 μm or less, and most preferably 5 to 20 μm. If the adhesive layer is too thick, scratch resistance will deteriorate, and if the adhesive layer is too thin, adhesion between the laminated glass and the reflective layer or transparent resin substrate will be insufficient, resulting in insufficient curved surface conformability.

[0199] From the viewpoint of scratch resistance, the adhesive layer preferably has a storage modulus E' at 25°C and a frequency of 1 Hz of greater than 1 kPa, and from the viewpoint of adhesion to the windshield, it is more preferably 4 GPa or less, even more preferably greater than 1 KPa and less than 1 GPa, and even more preferably greater than 1 KPa and less than 100 MPa.

[0200] The pressure-sensitive adhesive layer preferably has a maximum loss tangent (tan δ) at a frequency of 1 Hz in a temperature range of 40° C. to −80° C., more preferably 40° C. to −60° C. By setting tan δ within the above range, it is possible to achieve both excellent adhesion to laminated glass and durability.

[0201] In the present invention, the storage modulus and tan δ of the adhesive layer at a frequency of 1 Hz are determined as follows.

[0202] <Sample Preparation Method> The adhesive layer is dissolved or melted in a solvent to obtain a coating solution, which is then applied to the release-treated surface of a release-treated release PET sheet to a dry thickness of 40 μm, and dried. The adhesive layer is then peeled off from the release PET sheet to prepare a test piece for the adhesive layer. <Measurement Method> Using a dynamic viscoelasticity measuring device (DVA-225, manufactured by ITS Japan Co., Ltd.), the test piece is pre-conditioned for at least 2 hours at a temperature of 25°C and a relative humidity of 60%. Measurements are then performed under the following conditions in the "Step Temperature Ramp / Frequency Dispersion" mode. Then, using the "Master Curve" editor, master curves of tan δ, storage modulus, and loss modulus versus frequency at 25°C are obtained. The maximum value of tan δ and the frequency at which the maximum value is obtained are determined from the obtained master curve. Sample: 5 mm x 20 mm; Grip Distance: 20 mm; Set Strain: 0.10%; Measurement Temperature: -100°C to 40°C; Heating Condition: 2°C / min

[0203] (Method for forming adhesive layer) The method for forming the adhesive layer is not particularly limited, and examples thereof include a coating method, a casting method (solventless casting method and solvent casting method), a pressing method, an extrusion method, an injection molding method, a casting method, and an inflation method. In detail, an adhesive layer can be produced on a film by preparing a liquid product in which the adhesive layer material is dissolved or dispersed in a solvent, or a melt of the components constituting the adhesive layer material, and then applying this liquid product or melt to a film, and then removing the solvent as necessary.

[0204] Alternatively, an adhesive layer material can be applied to the release-treated surface of a release sheet that has been subjected to a release treatment in the same manner as described above, dried to form a sheet having an adhesive layer, and the adhesive layer of this sheet can be attached to a transparent resin substrate or a reflective layer to form an adhesive layer on the transparent resin substrate or the reflective layer.

[0205] (Protective film layer of adhesive layer) It is preferable to provide a peelable protective film layer on one side of the adhesive layer. By providing such a protective film layer, damage to the adhesive layer of the resin film before use and adhesion of dust, dirt, etc. can be prevented, and the protective film layer can be peeled off when used.

[0206] A release layer can be provided between the protective film layer and the adhesive layer to facilitate peeling of the protective film layer. The method for providing such a release layer is not particularly limited, and for example, the release layer can be provided by applying a release coating agent to the surface of at least one of the protective film layer and the adhesive layer. The type of release coating agent is not particularly limited, and examples thereof include silicone-based coating agents, inorganic-based coating agents, fluorine-based coating agents, and organic-inorganic hybrid coating agents.

[0207] A film comprising a protective film layer and a release layer can usually be obtained by providing a release layer on the surface of the protective film layer and then laminating it on the surface of the adhesive layer. In this case, the release layer may be provided on the surface of the adhesive layer instead of the surface of the protective film layer.

[0208] When a protective film layer is provided, it is preferable that the difference in thermal shrinkage between the protective film layer and the transparent resin substrate is small. Specifically, the difference in thermal shrinkage under heating conditions using a heat gun or the like in the curved surface conforming process is preferably 2.0% or less, more preferably 1.0% or less, and even more preferably 0.6% or less. By setting the difference in thermal shrinkage between the protective film layer and the transparent resin substrate within the above range, deformation of the transparent resin substrate during heating using a heat gun or the like to conform to the curved glass can be suppressed.

[0209] <Hard Coat Layer (HC Layer)> The laminated glass of the present invention may have a hard coat layer (HC layer). By having the HC layer, even in a configuration in which the transparent resin substrate is disposed on the outer side of the laminated glass, the HC layer protects the transparent resin substrate, thereby imparting abrasion resistance that makes it difficult to be scratched even when rubbed with a hard substance, scratch resistance that makes it difficult to be scratched even when pressed with a hard substance, and stain resistance that allows dirt to be easily wiped off even if dirt adheres to the glass.

[0210] The HC layer in the present invention is preferably obtained by polymerizing and curing at least one compound selected from the group consisting of polysiloxane-containing compounds having polymerizable groups in their molecules and fluorine-containing compounds having polymerizable groups in their molecules, and the polymerizable compound other than these compounds, which has polymerizable groups in its molecule as described below, and more preferably these polymerizable groups are radical polymerizable groups.Therefore, in the HC layer, the compound selected from the group consisting of polysiloxane-containing compounds and fluorine-containing compounds and the polymerizable compound forming the HC layer exist in a bonded state, and can provide better antifouling properties.When the compound selected from the group consisting of polysiloxane-containing compounds and fluorine-containing compounds has a polymerizable group, the polymerizable group in the compound selected from the group consisting of polysiloxane-containing compounds and fluorine-containing compounds described below will react to form a bond and exist in the HC layer.

[0211] In addition, when the HC layer has a laminated structure of two or more layers described later, the compound selected from the group consisting of a polysiloxane-containing compound and a fluorine-containing compound is preferably contained in at least the HC layer farthest from the adhesive layer, and more preferably contained only in the HC layer farthest from the adhesive layer. Specific embodiments of the HC layer will be described below, but the present invention is not limited to the following embodiments.

[0212] [Fluorine-containing compound] The fluorine-containing compound is not particularly limited as long as it can impart abrasion resistance and antifouling properties to the HC layer, and a compound having a fluorine atom in the molecule can be used. As the fluorine-containing compound, a fluorine-containing antifouling agent that exhibits the properties of an antifouling agent is preferably used.

[0213] The fluorine-containing compound may be any of a monomer, an oligomer, and a polymer. The fluorine-containing compound preferably has a substituent that contributes to bond formation or compatibility with other components in the HC layer (for example, a polysiloxane-containing compound, a polymerizable monomer that is a component of a resin, or a resin). The substituents may be the same or different, and it is preferable that there are a plurality of them. The substituent is preferably a polymerizable group, and may be any polymerizable reactive group that exhibits any of radical polymerization, cationic polymerization, anionic polymerization, condensation polymerization, and addition polymerization. Preferred examples of the substituent include an acryloyl group, a methacryloyl group, a vinyl group, an allyl group, a cinnamoyl group, an epoxy group, an oxetanyl group, a hydroxyl group, a polyoxyalkylene group, a carboxyl group, and an amino group. Among them, a radical polymerizable group is preferred, and an acryloyl group and a methacryloyl group are more preferred. The fluorine-containing compound may be a polymer or an oligomer with a compound that does not contain a fluorine atom.

[0214] The fluorine-containing antifouling agent is preferably a fluorine-based compound represented by the following general formula (F): f )-[(W)-(R A ) n ] m (In the formula, R f is a (per)fluoroalkyl group or a (per)fluoropolyether group, W is a single bond or a linking group, R Arepresents a polymerizable unsaturated group. n represents an integer of 1 to 3. m represents an integer of 1 to 3.

[0215] In general formula (F), R A represents a polymerizable unsaturated group. The polymerizable unsaturated group is preferably a group having an unsaturated bond that can undergo a radical polymerization reaction when irradiated with active energy rays such as ultraviolet rays or electron beams (i.e., a radically polymerizable group), and examples thereof include a (meth)acryloyl group, a (meth)acryloyloxy group, a vinyl group, and an allyl group. Of these groups, a (meth)acryloyl group, a (meth)acryloyloxy group, and groups in which any hydrogen atom is substituted with a fluorine atom are preferably used.

[0216] In general formula (F), R f represents a (per)fluoroalkyl group or a (per)fluoropolyether group. Here, the (per)fluoroalkyl group represents at least one of a fluoroalkyl group and a perfluoroalkyl group, and the (per)fluoropolyether group represents at least one of a fluoropolyether group and a perfluoropolyether group. From the viewpoint of antifouling properties, R f The higher the fluorine content in the polymer, the more preferable.

[0217] The (per)fluoroalkyl group is preferably a group having 1 to 20 carbon atoms, more preferably a group having 1 to 10 carbon atoms. The (per)fluoroalkyl group has a linear structure (for example, —CF 2 CF 3 , -CH 2 (CF 2 ) 4 H, —CH 2 (CF 2 ) 8 CF 3 , -CH 2 CH 2 (CF 2 ) 4 H), but also branched structures (e.g., —CH(CF 3 ) 2 , -CH 2 CF (CF 3 ) 2 , -CH(CH 3 )CF 2 CF 3, -CH(CH 3 ) (CF 2 ) 5 CF 2 H) or an alicyclic structure (preferably a 5- or 6-membered ring, such as a perfluorocyclohexyl group, a perfluorocyclopentyl group, or an alkyl group substituted with these groups).

[0218] The (per)fluoropolyether group refers to a (per)fluoroalkyl group having an ether bond, and may be a monovalent or divalent or higher valent group. Examples of the fluoropolyether group include -CH 2 OCH 2 CF 2 CF 3 , -CH 2 CH 2 OCH 2 C 4 F 8 H, —CH 2 CH 2 OCH 2 CH 2 C 8 F 17 , -CH 2 CH 2 OCF 2 CF 2 OCF 2 CF 2 H, and a fluorocycloalkyl group having 4 to 20 carbon atoms and 4 or more fluorine atoms. Examples of the perfluoropolyether group include -(CF 2 O) p -(CF 2 CF 2 O) q -, -[CF(CF 3 )CF 2 O] p -[CF(CF 3 )] q -, - (CF 2 CF 2 CF 2 O) p -, and -(CF 2 CF 2 O) pThe above-mentioned p and q each independently represent an integer of 0 to 20, provided that p+q is an integer of 1 or more. The total of p and q is preferably 1 to 83, more preferably 1 to 43, and even more preferably 5 to 23. From the viewpoint of excellent antifouling properties, the above-mentioned fluorine-containing antifouling agent is preferably -(CF 2 O) p -(CF 2 CF 2 O) q It is particularly preferred that the alkyl group has a perfluoropolyether group represented by the formula:

[0219] In the present invention, the fluorine-containing antifouling agent preferably has a perfluoropolyether group and a plurality of polymerizable unsaturated groups in one molecule.

[0220] In general formula (F), W represents a linking group. Examples of W include alkylene groups, arylene groups, and heteroalkylene groups, as well as linking groups formed by combining these groups. These linking groups may further include functional groups such as oxy groups, carbonyl groups, carbonyloxy groups, carbonylimino groups, and sulfonamide groups, as well as functional groups formed by combining these groups. W is preferably an ethylene group, and more preferably an ethylene group bonded to a carbonylimino group.

[0221] There are no particular restrictions on the fluorine atom content of the fluorine-containing antifouling agent, but it is preferably 20% by mass or more, more preferably 30 to 70% by mass, and even more preferably 40 to 70% by mass.

[0222] Preferred fluorine-containing antifouling agents include R-2020, M-2020, R-3833, M-3833 and Optool DAC (all trade names) manufactured by Daikin Chemical Industries, Ltd., and Megafac F-171, F-172, F-179A, RS-78, RS-90, Defensa MCF-300 and MCF-323 (all trade names) manufactured by Dainippon Ink Co., Ltd.

[0223] In light of abrasion resistance, in general formula (F), the product of n and m (n×m) is preferably 2 or greater, and more preferably 4 or greater.

[0224] In the case where n and m are simultaneously 1 in formula (F), specific examples of the preferred embodiment include the following formulae (F-1) to (F-3).

[0225] General formula (F-1): R f2 (CF 2 CF 2 ) p R 22 CH 2 CH 2 R 21 OCOCR 11 =CH 2

[0226] (In the formula, R f2 represents a fluorine atom or a fluoroalkyl group having 1 to 10 carbon atoms, and R 11 represents a hydrogen atom or a methyl group, and R 21 represents a single bond or an alkylene group, and R 22 represents a single bond or a divalent linking group, p is an integer representing the degree of polymerization, and the degree of polymerization p is k or more (k is an integer of 3 or more).

[0227] R 22 When represents a divalent linking group, examples of this divalent linking group include the same as those for W described above.

[0228] Examples of the fluorine atom-containing telomer type (meth)acrylate in the general formula (F-1) include partially or completely fluorinated alkyl ester derivatives of (meth)acrylic acid.

[0229] When the compound represented by the general formula (F-1) is synthesized by telomerization, the R group of the general formula (F-1) can be easily separated depending on the telomerization conditions and the separation conditions of the reaction mixture. f2 (CF 2 CF 2 ) p R 22 CH 2 CH 2 R 21 The compound may contain a plurality of fluorine-containing (meth)acrylic acid esters in which p in O- is k, k+1, k+2, . . .

[0230] General formula (F-2): F(CF 2 )q -CH 2 -CHX-CH 2 Y (wherein q is an integer of 1 to 20, X and Y are each a (meth)acryloyloxy group or a hydroxyl group, and at least one of X and Y is a (meth)acryloyloxy group).

[0231] The fluorine-containing (meth)acrylic acid ester represented by the general formula (F-2) has a trifluoromethyl group (—CF 3 Even a small amount of this fluorine-containing (meth)acrylic acid ester effectively orients the trifluoromethyl groups on the surface.

[0232] In view of abrasion resistance and ease of production of the compound, q is preferably 6 to 20, more preferably 8 to 10. A fluorine-containing (meth)acrylic acid ester having a fluoroalkyl group having 8 to 10 carbon atoms exhibits a superior effect of reducing the friction coefficient and is excellent in abrasion resistance, even compared with fluorine-containing (meth)acrylic acid esters having fluoroalkyl groups of other chain lengths.

[0233] Examples of the fluorine-containing (meth)acrylic acid ester represented by the general formula (F-2) include 1-(meth)acryloyloxy-2-hydroxy-4,4,5,5,6,6,7,7,8,8,9,9,10,10,11,11,12,12,13,13,13-heneicosafluorotridecane, 2-(meth)acryloyloxy-1-hydroxy-4,4,5,5,6,6,7,7,8,8,9,9,10,10,11,11,12,12,13,13,13-heneicosafluorotridecane, and 1,2-bis(meth)acryloyloxy-4,4,5,5,6,6,7,7,8,8,9,9,10,10,11,11,12,12,13,13,13-heneicosafluorotridecane. In the present invention, 1-acryloyloxy-2-hydroxy-4,4,5,5,6,6,7,7,8,8,9,9,10,10,11,11,12,12,13,13,13-heneicosafluorotridecane is preferred.

[0234] General formula (F-3): F(CF 2 ) r O (CF 2 CF2 O) s CF 2 CH 2 OCOCR 3 =CH 2 (In the formula R 3 represents a hydrogen atom or a methyl group, s represents an integer of 1 to 20, and r represents an integer of 1 to 4.

[0235] The fluorine atom-containing monofunctional (meth)acrylate represented by the above general formula (F-3) can be obtained by reacting a fluorine atom-containing alcohol compound represented by the following general formula (FG-3) with a (meth)acrylic acid halide.

[0236] General formula (FG-3): F(CF 2 ) r O (CF 2 CF 2 O) s CF 2 CH 2 OH (In general formula (FG-3), s represents an integer of 1 to 20, and r represents an integer of 1 to 4.)

[0237] Examples of the fluorine atom-containing alcohol compound represented by the general formula (FG-3) include 1H,1H-perfluoro-3,6-dioxaheptan-1-ol, 1H,1H-perfluoro-3,6-dioxaoctan-1-ol, 1H,1H-perfluoro-3,6-dioxadecan-1-ol, 1H,1H-perfluoro-3,6,9-trioxadecan-1-ol, 1H,1H-perfluoro-3,6,9-trioxaundecan-1-ol, 1H,1H-perfluoro-3,6,9-trioxatridecan-1-ol, 1H,1H-perfluoro-3,6,9,12-tetraoxatridecan-1-ol, 1H,1H-perfluoro-3,6,9,12-tetraoxatetradecan-1-ol, and 1H,1H-perfluoro-3,6,9,12-tetraoxatetradecan-1-ol. Oxahexadecan-1-ol, 1H,1H-perfluoro-3,6,9,12,15-pentaoxahexadecan-1-ol, 1H,1H-perfluoro-3,6,9,12,15-pentaoxaheptadecan-1-ol, 1H,1H-perfluoro-3,6,9,12,15-pentaoxanonadecan-1-ol, 1H,1H-perfluoro-3,6,9,12,15,1 8-hexaoxaicosan-1-ol, 1H,1H-perfluoro-3,6,9,12,15,18-hexaoxadocosan-1-ol, 1H,1H-perfluoro-3,6,9,12,15,18,21-heptaoxatricosan-1-ol, and 1H,1H-perfluoro-3,6,9,12,15,18,21-heptaoxapentacosan-1-ol.These are commercially available products, and specific examples thereof include 1H,1H-perfluoro-3,6-dioxaheptan-1-ol (trade name "C5GOL", manufactured by Exflo Corporation), 1H,1H-perfluoro-3,6,9-trioxadecan-1-ol (trade name "C7GOL", manufactured by Exflo Corporation), 1H,1H-perfluoro-3,6-dioxadecan-1-ol (trade name "C8GOL", manufactured by Exflo Corporation), 1H,1H-perfluoro-3,6,9-trioxatridecan-1-ol (trade name "C10GOL", manufactured by Exflo Corporation), and 1H,1H-perfluoro-3,6,9,12-tetraoxahexadecan-1-ol (trade name "C12GOL", manufactured by Exflo Corporation). In the present invention, it is preferable to use 1H,1H-perfluoro-3,6,9,12-tetraoxatridecan-1-ol.

[0238] Examples of the (meth)acrylic acid halide to be reacted with the fluorine atom-containing alcohol compound represented by general formula (FG-3) include (meth)acrylic acid fluoride, (meth)acrylic acid chloride, (meth)acrylic acid bromide, and (meth)acrylic acid iodide. From the viewpoint of availability, etc., (meth)acrylic acid chloride is preferred.

[0239] Preferable specific examples of the compound represented by general formula (F-3) are shown below, but the compound is not limited to these. Preferable specific examples represented by general formula (F-3) are also described in JP-A-2007-264221.

[0240] (b-1): F 9 C 4 O.C. 2 F 4 O.C. 2 F 4 OCF 2 CH 2 OCOCH=CH 2 (b-2): F 9 C 4 O.C. 2 F 4 O.C. 2 F 4 OCF 2 CH 2 OCOC (CH3 ) = CH 2

[0241] Furthermore, in addition to the compound represented by formula (F-3), a compound represented by the following formula (F-3)' can also be preferably used.

[0242] General formula (F-3)': R f3 - [(O) c (O=C) b (CX 4 X 5 ) a -CX 3 =CX 1 X 2 ] (In the formula, X 1 and X 2 represents H or F, and X 3 are H, F, and CH 3 or CF 3 represents X 4 and X 5 is H, F, or CF 3 a, b, and c represent 0 or 1; R f3 represents a fluorine-containing organic group containing an ether bond and having 18 to 200 carbon atoms.) The compound represented by the general formula (F-3)' is f3 In the group, the general formula (FG-3)': -(CX 6 2 CF 2 CF 2 O)-(wherein, X 6 is a fluorine-containing unsaturated compound having six or more repeating units represented by F or H).

[0243] Examples of the fluorine-containing polyether compound represented by the general formula (F-3)' include: f3 -[(O) (O=C) b -CX 3 =CX 1 X 2 ] (c-2) R f3 -[(O)(O=C)-CX 3 =CX 1 X 2 ] (c-3) R f3 - [(O) c (O=C)-CF=CH 2(The definition of each symbol in (c-1) to (c-3) is the same as in formula (FG-3)'.) As the polymerizable unsaturated group of the above fluorine-containing polyether compound, those having the following structure can be preferably used.

[0244] The fluorine-containing polyether compound represented by the general formula (F-3)' may have a plurality of polymerizable unsaturated groups. 2 Compounds having the following structure are preferred in that they have particularly high polymerization (curing) reactivity and can efficiently produce cured products.

[0245] The fluorine-containing polyether compound represented by the general formula (F-3)′ is R f3 It is important that the group contains 6 or more repeating units of the fluorine-containing polyether chain represented by general formula (FG-3)', thereby imparting abrasion resistance. More specifically, a mixture containing 6 or more repeating units of the fluorine-containing polyether chain may be used, and when used in the form of a mixture, it is preferable to use a mixture in which the abundance ratio of fluorine-containing unsaturated compounds having 6 or more repeating units of the polyether chain is highest in the distribution of the fluorine-containing unsaturated compounds having less than 6 repeating units and the fluorine-containing unsaturated compounds having 6 or more repeating units. The number of repeating units of the fluorine-containing polyether chain represented by general formula (FG-3)' is preferably 6 or more, more preferably 10 or more, even more preferably 18 or more, and particularly preferably 20 or more. This reduces the coefficient of dynamic friction and improves abrasion resistance. Furthermore, the fluorine-containing polyether chain R f3 It may be at the end of the group or in the chain.

[0246] R f3 Specifically, the group is represented by the general formula (c-4): R 4 - (CX 6 2 CF 2 CF 2 O) t - (R 5 ) e - (wherein, X 6 is X in the fluorine-containing polyether chain represented by formula (FG-3)' 6is synonymous with R 4 is a hydrogen atom, a halogen atom, an alkyl group, a fluorine-containing alkyl group, an alkyl group containing an ether bond or a fluorine-containing alkyl group containing an ether bond, R 5 is a divalent or higher organic group, t is an integer of 6 to 66, and e is 0 or 1. f3 The group is a divalent or higher organic group R 5 and further has R at the end. 4 R is a fluorine-containing organic group having the formula 5 may be any organic group capable of bonding the fluorine-containing polyether chain represented by general formula (FG-3)' to a reactive carbon-carbon double bond. Examples thereof include an alkylene group, a fluorine-containing alkylene group, an alkylene group containing an ether bond, and a fluorine-containing alkylene group containing an ether bond. Among these, a fluorine-containing alkylene group and a fluorine-containing alkylene group containing an ether bond are preferred in terms of transparency and a low refractive index.

[0247] As specific examples of the fluorine-containing polyether compound represented by the general formula (F-3)′, compounds such as those described in the republished patent publication WO2003 / 022906 are preferably used. 2 =CF-COO-CH 2 CF 2 CF 2 -(OCF 2 CF 2 CF 2 ) 7 -OC 3 F 7 can be particularly preferably used.

[0248] In the case where n and m are not 1 at the same time in formula (F), the following preferred embodiments include formulae (F-4) and (F-5).

[0249] General formula (F-4): (R f1 )-[(W)-(R A ) n ] m (In general formula (F-4), R f1is a (per)fluoroalkyl group or a (per)fluoropolyether group, W is a linking group, R A represents a polymerizable unsaturated group. n represents an integer of 1 to 3, and m represents an integer of 1 to 3, provided that n and m are not simultaneously 1.) From the viewpoint of achieving excellent water and oil repellency and excellent sustainability of the water and oil repellency (soil-resistant durability), it is preferable that n is 2 to 3 and m is 1 to 3, more preferably that n is 2 to 3 and m is 2 to 3, and even more preferably that n is 3 and m is 2 to 3.

[0250] R f1 R can be monovalent to trivalent. f1 When is monovalent, the terminal group is (C n F 2n+1 ) -, (C n F 2n+1 O) -, (XC n F 2n O) -, (XC n F 2n+1 )-(wherein X is a hydrogen atom, a chlorine atom, or a bromine atom, and n is an integer of 1 to 10). 3 O (C 2 F 4 O) p CF 2 -, C 3 F 7 O (CF 2 CF 2 CF 2 O) p CF 2 CF 2 -, C 3 F 7 O(CF(CF 3 )CF 2 O) p CF (CF 3 )-, or F(CF(CF 3 )CF 2 O) p CF (CF 3 )- is preferred.

[0251] Here, the average value of p is 0 to 50, preferably 3 to 30, more preferably 3 to 20, and even more preferably 4 to 15.

[0252] R f1 If is divalent, -(CF2 O) q (C 2 F 4 O) r CF 2 -, - (CF 2 ) 3 O (C 4 F 8 O) r (CF 2 ) 3 -, -CF 2 O (C 2 F 4 O) r CF 2 -, -C 2 F 4 O (C 3 F 6 O) r C 2 F 4 -, -CF(CF 3 ) (OCF 2 CF (CF 3 )) s O.C. t F 2t O(CF(CF 3 )CF 2 O) r CF (CF 3 ) - or -(CF(CF 3 )CF 2 O) p CF (CF 3 )- is preferred.

[0253] Here, the average values ​​of p, q, r, and s in the formula are 0 to 50, preferably 3 to 30, more preferably 3 to 20, and even more preferably 4 to 15. t is an integer of 2 to 6. Preferred specific examples and synthesis methods of the compound represented by general formula (F-4) are described in WO 2005 / 113690.

[0254] In the following, F(CF(CF 3 )CF 2 O) p CF (CF 3 )-, those with an average value of p of 6 to 7 are described as "HFPO-", and -(CF(CF 3 )CF 2 O) p CF (CF 3)--wherein the average value of p is 6 to 7 is expressed as "-HFPO--", and specific compounds of general formula (F-4) are shown, but are not limited to these.

[0255] (d-1): HFPO-CONH-C-(CH 2 OCOCH=CH 2 ) 2 CH 2 CH 3 (d-2): HFPO-CONH-C-(CH 2 OCOCH=CH 2 ) 2 H (d-3): HFPO-CONH-C 3 H 6 NHCH 3 1:1 Michael addition polymer of trimethylolpropane triacrylate (d-4): (CH 2 =CHCOOCH 2 ) 2 HC-CONH-HFPO-CONH-(CH 2 OCOCH=CH 2 ) 2 H (d-5): (CH 2 =CHCOOCH 2 ) 3 -C-CONH-HFPO-CONH-C-(CH 2 OCOCH=CH 2 ) 3

[0256] Furthermore, as the compound represented by general formula (F-4), a compound represented by the following general formula (F-5) can also be used.

[0257] General formula (F-5): CH 2 =CX 1 -COO-CHY-CH 2 -OCO-CX 2 =CH 2 (X in the formula 1 and X 2 represents a hydrogen atom or a methyl group, and Y represents a fluoroalkyl group having 2 to 20 carbon atoms and 3 or more fluorine atoms, or a fluorocycloalkyl group having 4 to 20 carbon atoms and 4 or more fluorine atoms.

[0258] The compound in which the polymerizable unsaturated group is a (meth)acryloyloxy group may have a plurality of (meth)acryloyloxy groups. When the fluorine-containing antifouling agent has a plurality of (meth)acryloyloxy groups, it forms a three-dimensional network structure when cured, has a high glass transition temperature, has low transferability of the antifouling agent, and can improve durability against repeated wiping of stains. Furthermore, it can obtain an HC layer excellent in heat resistance, weather resistance, etc.

[0259] Examples of the compound represented by the general formula (F-5) include 2,2,2-trifluoroethylethylene glycol di(meth)acrylate, 2,2,3,3,3-pentafluoropropylethylene glycol di(meth)acrylate, 2,2,3,3,4,4,4-heptafluorobutylethylene glycol di(meth)acrylate, 2,2,3,3,4,4,5,5,5-nonafluoropentylethylene glycol di(meth)acrylate, 2,2,3,3,4, 4,5,5,6,6,6-undecafluorohexylethylene glycol, 2,2,3,3,4,4,5,5,6,6,7,7,7-tridecafluoroheptylethylene glycol di(meth)acrylate, 2,2,3,3,4,4,5,5,6,6,7,7,8,8,8-pentadecafluorooctylethylene glycol di(meth)acrylate, 3,3,4,4,5,5,6,6,7,7,8,8,8-tridecafluorooctylethylene glycol di(meth)acrylate, ) 2,2,3,3,4,4,5,5,6,6,7,7,8,8,9,9,9-heptadecafluorononylethylene glycol acrylate, 2,2,3,3,4,4,5,5,6,6,7,7,8,8,9,9,10,10,10-nonadecafluorodecylethylene glycol di(meth)acrylate, 3,3,4,4,5,5,6,6,7,7,8,8,9,9,10,10,10-heptadecafluorodecylethylene glycol di(meth)acrylate, 2-(2-methyl-2-propanol)-2-propanol Examples of di(meth)acrylates include 3,3,3-trifluoromethyl-3,3,3-trifluoropropylethylene glycol, 3-trifluoromethyl-4,4,4-trifluorobutylethylene glycol di(meth)acrylate, 1-methyl-2,2,3,3,3-pentafluoropropylethylene glycol di(meth)acrylate, and 1-methyl-2,2,3,3,4,4,4-heptafluorobutylethylene glycol di(meth)acrylate, and these can be used alone or in combination. Such di(meth)acrylic acid esters can be prepared by known methods such as those described in JP-A-6-306326.In the present invention, 2,2,3,3,4,4,5,5,6,6,7,7,8,8,9,9,9-heptadecafluorononylethylene glycol diacrylate is preferably used.

[0260] In the present invention, the compound in which the polymerizable unsaturated group is a (meth)acryloyloxy group may be a compound having a plurality of (per)fluoroalkyl groups or (per)fluoropolyether groups in one molecule.

[0261] (Molecular Weight of Fluorine-Containing Compound) The weight-average molecular weight (Mw) of a fluorine-containing compound having a polymerizable unsaturated group can be measured using molecular exclusion chromatography, such as gel permeation chromatography (GPC). The Mw of the fluorine-containing compound is preferably 400 or more and less than 50,000, more preferably 400 or more and less than 30,000, and even more preferably 400 or more and less than 25,000. If it is equal to or greater than the lower limit, the surface migration of the antifouling agent in the HC layer is enhanced, which is preferable. If it is less than the upper limit, the surface migration of the fluorine-containing compound is not hindered during the process of applying and curing the curable composition for forming an HC layer, which makes it easier for the fluorine-containing compound to be unevenly distributed on the HC layer surface, which is preferable, and improves the abrasion resistance and film hardness. In addition, the fluorine-containing compound may have a multimodal weight-average molecular weight.

[0262] (Amount of Fluorine-Containing Compound Added) The amount of fluorine-containing compound added is preferably 0.01 to 5 mass%, more preferably 0.1 to 5 mass%, even more preferably 0.5 to 5 mass%, and particularly preferably 0.5 to 2 mass%, relative to the total solids content in the curable composition for forming an HC layer. When the amount added is equal to or greater than the above upper limit, the coefficient of friction can be reduced, and abrasion resistance is further improved. Furthermore, when the amount added is equal to or less than the above lower limit, fluorine-containing compounds that are insufficiently mixed with the polymerizable compound in the curable composition for forming an HC layer (the resin component when forming the HC layer) do not precipitate on the surface, which is preferable because it prevents the HC layer from whitening or the generation of white powder on the surface. Note that when the HC layer has a laminate structure of two or more layers, as described below, this refers to the amount added in the curable composition for forming an HC layer that forms an HC layer containing a fluorine-containing compound or a polysiloxane compound.

[0263] [Polysiloxane-containing compound] The polysiloxane-containing compound is not particularly limited, and a compound having a polysiloxane structure in the molecule can be used. The polysiloxane structure of the polysiloxane-containing compound may be any of linear, branched, and cyclic. As the polysiloxane-containing compound, a polysiloxane antifouling agent exhibiting the properties of an antifouling agent is preferably used.

[0264] The polysiloxane antifouling agent is preferably a compound represented by the following general formula (F-6).

[0265] General formula (F-6): R a R A b SiO (4-a-b)/2 (wherein R is a hydrogen atom, a methyl group, an ethyl group, a propyl group, or a phenyl group; R A is an organic group containing a polymerizable unsaturated group, and 0<a, 0<b, a+b<4.

[0266] a is preferably 1 to 2.75, more preferably 1 to 2.5. When a is 1 or more, the compound can be easily synthesized industrially, and when it is 2.75 or less, both curability and antifouling properties can be easily achieved.

[0267] R A As the polymerizable unsaturated group in the general formula (F), R A Examples of the polymerizable unsaturated groups (i.e., radically polymerizable groups) include those similar to those mentioned above, and are preferably a (meth)acryloyl group, a (meth)acryloyloxy group, and groups in which any hydrogen atom in these groups has been substituted with a fluorine atom. In terms of film strength, the polysiloxane antifouling agent also preferably has a plurality of polymerizable unsaturated groups in one molecule, and is more preferably a polydimethylsiloxane having a plurality of polymerizable unsaturated groups in one molecule.

[0268] Preferred examples of polysiloxane antifouling agents include those having a substituent at the end and / or side chain of a compound chain containing multiple dimethylsilyloxy units as repeating units. The compound chain containing dimethylsilyloxy as a repeating unit may contain structural units other than dimethylsilyloxy. These substituents may be the same or different, and preferably there are multiple substituents. This substituent is preferably a polymerizable group, and may be any polymerizable group exhibiting radical polymerization, cationic polymerization, anionic polymerization, condensation polymerization, or addition polymerization. Preferred examples of the substituent include groups containing a (meth)acryloyl group, a ((meth)acryloyloxy) group, a vinyl group, an allyl group, a cinnamoyl group, an epoxy group, an oxetanyl group, a hydroxyl group, a fluoroalkyl group, a polyoxyalkylene group, a carboxyl group, or an amino group. Of these, radical polymerizable groups are preferred, and a (meth)acryloyloxy group is preferred from the viewpoint of improving antifouling properties. Furthermore, from the viewpoint of achieving both film strength and antifouling properties, the number of the above-mentioned substituents in the compound is preferably 100 to 10,000 g / mol in terms of functional group equivalent, more preferably 100 to 3,000 g / mol, even more preferably 100 to 2,000 g / mol, and particularly preferably 100 to 1,000 g / mol. By making the functional group equivalent equal to or greater than the above-mentioned lower limit, the compound is not more compatible with the polymerizable compound in the curable composition for forming the HC layer (the resin component when forming the HC layer), which is preferable because it increases the surface migration of the antifouling agent in the HC layer. By making the functional group equivalent equal to or less than the above-mentioned upper limit, it is preferable because it can improve film hardness and antifouling properties.

[0269] R A is preferably an organic group containing a (meth)acryloyl group, and from the viewpoint of ease of industrial synthesis, it is more preferable that the bond to the Si atom be an Si—O—C bond. b is preferably 0.4 to 0.8, more preferably 0.6 to 0.8. When b is equal to or greater than the lower limit, curability is improved, and when it is equal to or less than the upper limit, antifouling properties are improved.

[0270] Furthermore, a+b is preferably 3 to 3.7, and more preferably 3 to 3.5. If it is equal to or greater than the lower limit, the compound is likely to be unevenly distributed on the surface of the HC layer, whereas if it is equal to or less than the upper limit, both curability and antifouling properties can be improved.

[0271] The polysiloxane antifouling agent preferably has 3 or more Si atoms in one molecule, and more preferably 3 to 40 Si atoms. When there are 3 or more Si atoms, the compound is more likely to be unevenly distributed on the HC layer surface, making it easier to obtain sufficient antifouling properties.

[0272] The polysiloxane antifouling agent can be produced by a known method such as that described in JP-A-2007-145884. Examples of additives having a polysiloxane structure include polysiloxanes (e.g., "KF-96-10CS", "KF-100T", "X-22-169AS", "KF-102", "X-22-3701IE", "X-22-164", "X-22-164A", "X-22-164AS", "X-22-164B", "X-22-164C", "X-22-5002", "X-22-173B", "X-22-174D", "X-22-167 ... It is also preferable to add "61AS" (trade name), all manufactured by Shin-Etsu Chemical Co., Ltd.; "AK-5", "AK-30", "AK-32" (trade names), all manufactured by Toagosei Co., Ltd.; "Silaplane FM0725" and "Silaplane FM0721" (trade names), all manufactured by Chisso Corporation; "DMS-U22", "RMS-033", "UMS-182" (trade names), all manufactured by Gelest; "Acrit 8SS-723" (trade name), all manufactured by Taisei Fine Chemical Co., Ltd.). Also preferred are the polysiloxane compounds described in Tables 2 and 3 of JP-A No. 2003-112383.

[0273] [Molecular Weight of Polysiloxane-Containing Compound] The weight-average molecular weight of the polysiloxane-containing compound is preferably 300 or more, more preferably 300 to 100,000, and even more preferably 300 to 30,000. When the weight-average molecular weight of the polysiloxane-containing compound is 300 or more, uneven distribution of the polysiloxane-containing compound on the surface of the HC layer is promoted, and the abrasion resistance and hardness are further improved.

[0274] [Amount of Polysiloxane-Containing Compound Added] The amount of polysiloxane-containing compound added is preferably 0.01 to 5 mass%, more preferably 0.1 to 5 mass%, even more preferably 0.5 to 5 mass%, and particularly preferably 0.5 to 2 mass%, relative to the total solids content in the curable composition for forming an HC layer. When the amount added is equal to or greater than the lower limit, the antifouling properties can be further improved. Furthermore, when the amount added is equal to or less than the upper limit, the polysiloxane-containing compound that is insufficiently mixed with the polymerizable compound in the curable composition for forming an HC layer (the resin component when forming the HC layer) does not precipitate on the surface, which is preferable because it prevents the HC layer from whitening or the generation of white powder on the surface. Note that when the HC layer has a laminate structure of two or more layers, as described below, this refers to the amount added in the curable composition for forming an HC layer that contains the polysiloxane compound.

[0275] (HC layer obtained by curing a curable composition for forming a hard coat layer (HC layer)) The HC layer used in the present invention can be obtained by irradiating an HC layer-forming curable composition with active energy rays and curing it. In this specification, the term "active energy rays" refers to ionizing radiation, and includes X-rays, ultraviolet rays, visible light, infrared rays, electron beams, α rays, β rays, γ rays, etc.

[0276] The curable composition for forming the HC layer used to form the HC layer contains at least one component that has the property of being cured by irradiation with active energy rays (hereinafter also referred to as "active energy ray-curable component"). The active energy ray-curable component is preferably at least one polymerizable compound selected from the group consisting of radically polymerizable compounds and cationically polymerizable compounds. In this specification, "polymerizable compound" refers to a compound having a polymerizable group in its molecule, and there may be at least one polymerizable group per molecule. The polymerizable group is a group that can participate in a polymerization reaction, and specific examples include groups contained in various polymerizable compounds described below. Examples of the polymerization reaction include various polymerization reactions such as radical polymerization, cationic polymerization, and anionic polymerization. The HC layer of the present invention is preferably obtained by irradiating a curable composition for forming the HC layer, which contains at least one compound selected from the group consisting of polysiloxane-containing compounds having a polymerizable group in their molecules and fluorine-containing compounds having a polymerizable group in their molecules, and a polymerizable compound other than these compounds having a polymerizable group in their molecules, with active energy rays to polymerize and cure the composition. In this case, the polymerizable groups possessed by the polysiloxane-containing compound, the fluorine-containing compound, and the polymerizable compound are more preferably radically polymerizable groups. The HC layer used in the present invention may have a single-layer structure or a laminated structure of two or more layers, and an HC layer having a single-layer structure or a laminated structure of two or more layers, which will be described in detail below, is preferred.

[0277] 1) Single-Layer Structure As a preferred embodiment of the single-layer structure curable composition for forming an HC layer, a first embodiment is a curable composition for forming an HC layer containing at least one polymerizable compound having two or more ethylenically unsaturated groups in one molecule. The ethylenically unsaturated group refers to a functional group containing an ethylenically unsaturated double bond. A second embodiment is a curable composition for forming an HC layer containing at least one radically polymerizable compound and at least one cationically polymerizable compound.

[0278] The curable composition for forming an HC layer of the first embodiment will be described below. Examples of the polymerizable compound having two or more ethylenically unsaturated groups in one molecule contained in the curable composition for forming an HC layer of the first embodiment include esters of polyhydric alcohols and (meth)acrylic acid [for example, ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, 1,4-cyclohexane diacrylate, pentaerythritol tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta ... (meth)acrylate, dipentaerythritol hexa(meth)acrylate, pentaerythritol hexa(meth)acrylate, 1,2,3-cyclohexane tetramethacrylate, polyurethane polyacrylate, polyester polyacrylate], ethylene oxide modified products, polyethylene oxide modified products and caprolactone modified products of the above esters, vinylbenzene and derivatives thereof [e.g., 1,4-divinylbenzene, 4-vinylbenzoic acid-2-acryloylethyl ester, 1,4-divinylcyclohexanone], vinyl sulfones (e.g., divinyl sulfone), acrylamides (e.g., methylenebisacrylamide) and methacrylamide.

[0279] The polymerization of the polymerizable compound having an ethylenically unsaturated group can be carried out by irradiation with active energy rays in the presence of a radical photopolymerization initiator.As the radical photopolymerization initiator, the radical photopolymerization initiator described later is preferably used.In addition, with regard to the content ratio of the radical photopolymerization initiator to the polymerizable compound having an ethylenically unsaturated group in the curable composition for forming an HC layer, the content ratio of the radical photopolymerization initiator to the radical polymerizable compound described later is preferably used.

[0280] Next, the curable composition for forming an HC layer of the second embodiment will be described. The curable composition for forming an HC layer of the second embodiment preferably contains at least one radical polymerizable compound and at least one cationic polymerizable compound. A preferred embodiment can include a curable composition for forming an HC layer comprising: a radical polymerizable compound containing two or more radical polymerizable groups selected from the group consisting of acryloyl groups and methacryloyl groups in one molecule; and a cationic polymerizable compound.

[0281] The curable composition for forming the HC layer preferably contains a radical photopolymerization initiator and a cationic photopolymerization initiator. A preferred embodiment of the second aspect is a curable composition for forming the HC layer, which comprises: a radical polymerizable compound containing two or more radical polymerizable groups selected from the group consisting of acryloyl groups and methacryloyl groups per molecule; a cationic polymerizable compound; a radical photopolymerization initiator; and a cationic photopolymerization initiator. Hereinafter, this embodiment will be referred to as the second aspect (1).

[0282] In the second aspect (1), the radically polymerizable compound preferably contains two or more radically polymerizable groups in one molecule and one or more urethane bonds in one molecule.

[0283] Another preferred embodiment of the second embodiment is a curable composition for forming an HC layer, comprising: a) a cationically polymerizable compound containing an alicyclic epoxy group and an ethylenically unsaturated group, wherein the compound contains one alicyclic epoxy group and one ethylenically unsaturated group per molecule, and has a molecular weight of 300 or less; b) a radically polymerizable compound containing three or more ethylenically unsaturated groups per molecule; c) a radical polymerization initiator; and d) a cationic polymerization initiator. Hereinafter, this embodiment will be referred to as Second Aspect (2). The HC layer obtained by curing the curable composition for forming an HC layer of Second Aspect (2) can preferably contain, relative to the total solids content of the HC layer being 100% by mass, 15 to 70% by mass of the structure derived from a) above, 25 to 80% by mass of the structure derived from b) above, 0.1 to 10% by mass of c) above, and 0.1 to 10% by mass of d) above. In one embodiment, the curable composition for forming an HC layer of the second embodiment (2) preferably contains 15 to 70 mass% of the above-mentioned a) when the total solid content of the curable composition for forming an HC layer is taken as 100 mass%. The term "alicyclic epoxy group" refers to a monovalent functional group having a cyclic structure in which an epoxy ring and a saturated hydrocarbon ring are condensed.

[0284] Hereinafter, various components that can be contained in the curable composition for forming an HC layer according to the second embodiment, preferably the second embodiment (1) or the second embodiment (2), will be described in more detail.

[0285] -Radical polymerizable compound- The curable composition for forming an HC layer of the second embodiment contains at least one radically polymerizable compound and at least one cationically polymerizable compound. The radically polymerizable compound in the second embodiment (1) contains two or more radically polymerizable groups selected from the group consisting of acryloyl groups and methacryloyl groups per molecule. The radically polymerizable compound preferably contains 2 to 10, and more preferably 2 to 6, radically polymerizable groups selected from the group consisting of acryloyl groups and methacryloyl groups per molecule.

[0286] The radical polymerizable compound is preferably a radical polymerizable compound having a molecular weight of 200 or more and less than 1,000. In addition, the "molecular weight" refers to the weight average molecular weight of a polymer measured in terms of polystyrene by gel permeation chromatography (GPC). Specific measurement conditions for the weight average molecular weight include the following, for example: GPC apparatus: HLC-8120 (manufactured by Tosoh Corporation) Column: TSKgelMultiporeHXL-M (manufactured by Tosoh Corporation, inner diameter 7.8 mm x column length 30.0 cm) Eluent: tetrahydrofuran

[0287] Furthermore, the curable composition for forming an HC layer of the second aspect (1) may contain, in addition to a radical polymerizable compound containing two or more radical polymerizable groups selected from the group consisting of acryloyl groups and methacryloyl groups in one molecule, one or more radical polymerizable compounds other than the radical polymerizable compound.

[0288] Hereinafter, a radical polymerizable compound that contains two or more radical polymerizable groups selected from the group consisting of acryloyl groups and methacryloyl groups in one molecule and does not fall under the category of a first radical polymerizable compound will be referred to as a “second radical polymerizable compound.” When the first radical polymerizable compound and the second radical polymerizable compound are used in combination, the mass ratio thereof (first radical polymerizable compound / second radical polymerizable compound) is preferably 3 / 1 to 1 / 30, more preferably 2 / 1 to 1 / 20, and even more preferably 1 / 1 to 1 / 10.

[0289] The content of the radical polymerizable compound containing two or more radical polymerizable groups selected from the group consisting of acryloyl groups and methacryloyl groups in one molecule in the curable composition for forming an HC layer of the second aspect (1) is preferably 30% by mass or more, more preferably 50% by mass or more, and even more preferably 70% by mass or more, relative to 100% by mass of the total amount of the composition. Furthermore, the content of the radical polymerizable compound containing two or more radical polymerizable groups selected from the group consisting of acryloyl groups and methacryloyl groups in one molecule in the curable composition for forming an HC layer of the second aspect (1) is preferably 98% by mass or less, more preferably 95% by mass or less, and even more preferably 90% by mass or less, relative to 100% by mass of the total amount of the composition. Furthermore, the content of the first radical polymerizable compound in the curable composition for forming an HC layer of the second aspect (1) is preferably 30% by mass or more, more preferably 50% by mass or more, and even more preferably 70% by mass or more, relative to 100% by mass of the total amount of the composition. On the other hand, the content of the first radically polymerizable compound is preferably 98% by mass or less, more preferably 95% by mass or less, and even more preferably 90% by mass or less, relative to 100% by mass of the total amount of the composition.

[0290] Examples of the second radically polymerizable compound include the following: However, the present invention is not limited to the following exemplary compounds.

[0291] For example, polyethylene glycol 200 di(meth)acrylate, polyethylene glycol 300 di(meth)acrylate, polyethylene glycol 400 di(meth)acrylate, polyethylene glycol 600 di(meth)acrylate, triethylene glycol di(meth)acrylate, epichlorohydrin-modified ethylene glycol di(meth)acrylate (commercially available products include Denacol DA-811 manufactured by Nagase & Co., Ltd.), polypropylene glycol 200 di(meth)acrylate, polypropylene glycol 400 di(meth)acrylate, polypropylene glycol 700 di(meth)acrylate, ethylene oxide (EO), propylene oxide (PO),Examples of suitable polyether di(meth)acrylates include dipropylene glycol di(meth)acrylate, bisphenol AEO adduct di(meth)acrylate (commercially available products include, for example, the Blemmer PET series manufactured by Nippon Oil & Fats Co., Ltd.), dipropylene glycol di(meth)acrylate, bisphenol AEO adduct di(meth)acrylate (commercially available products include, for example, M-210 manufactured by Toagosei Co., Ltd. and NK Ester A-BPE-20 manufactured by Shin-Nakamura Chemical Co., Ltd.), and hydrogenated bisphenol AEO adduct di(meth)acrylate (commercially available products include, for example, M-210 manufactured by Toagosei Co., Ltd. and NK Ester A-BPE-20 manufactured by Shin-Nakamura Chemical Co., Ltd.). NK Ester A-HPE-4 manufactured by Kyoeisha Chemical Co., Ltd., etc.), bisphenol APO adduct di(meth)acrylate (commercially available products, for example, Light Acrylate BP-4PA manufactured by Kyoeisha Chemical Co., Ltd., etc.), bisphenol A epichlorohydrin adduct di(meth)acrylate (commercially available products, for example, Ebecryl 150 manufactured by Daicel UCB, etc.), bisphenol A EO·PO adduct di(meth)acrylate (commercially available products, for example, BP-023-PE manufactured by Toho Chemical Industry Co., Ltd., etc.), bis Examples of bifunctional (meth)acrylate compounds include phenol FEO addition type di(meth)acrylate (commercially available products include Aronix M-208 manufactured by Toagosei Co., Ltd.), 1,6-hexanediol di(meth)acrylate and epichlorohydrin-modified products thereof, neopentyl glycol di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate and caprolactone-modified products thereof, 1,4-butanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, trimethylolpropane di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, pentaerythritol di(meth)acrylate monostearate, trimethylolpropane acrylic acid benzoate, and isocyanuric acid EO-modified di(meth)acrylate (commercially available products include Aronix M-215 manufactured by Toagosei Co., Ltd.);

[0292] Further, trifunctional (meth)acrylate compounds such as trimethylolpropane tri(meth)acrylate (commercially available products include TPMTA manufactured by Nippon Kayaku Co., Ltd.) and its EO, PO, or epichlorohydrin-modified products, pentaerythritol tri(meth)acrylate, glycerol tri(meth)acrylate and its EO, PO, or epichlorohydrin-modified products, isocyanuric acid EO-modified tri(meth)acrylate (commercially available products include Aronix M-315 manufactured by Toagosei Co., Ltd.), tris(meth)acryloyloxyethyl phosphate, hydrogen phthalate-(2,2,2-tri-(meth)acryloyloxymethyl)ethyl, glycerol tri(meth)acrylate and its EO, PO, or epichlorohydrin-modified products; Examples of the second radical polymerizable compound include tetrafunctional (meth)acrylate compounds such as dipentaerythritol tetra(meth)acrylate (e.g., TPMTA manufactured by Shin-Nakamura Chemical Co., Ltd.), EO-, PO-, or epichlorohydrin-modified products thereof, and ditrimethylolpropane tetra(meth)acrylate; pentafunctional (meth)acrylate compounds such as dipentaerythritol penta(meth)acrylate, and EO-, PO-, epichlorohydrin-, fatty acid-, or alkyl-modified products thereof; and hexafunctional (meth)acrylate compounds such as dipentaerythritol hexa(meth)acrylate, and EO-, PO-, epichlorohydrin-, fatty acid-, or alkyl-modified products thereof, and sorbitol hexa(meth)acrylate, and EO-, PO-, epichlorohydrin-, fatty acid-, or alkyl-modified products thereof. Two or more types of the second radical polymerizable compound may be used in combination. In this case, a mixture of dipentaerythritol pentaacrylate and dipentaerythritol hexaacrylate, "DPHA" (manufactured by Nippon Kayaku Co., Ltd.), or the like can be preferably used.

[0293] Also preferred as the second radical polymerizable compound are polyester(meth)acrylates and epoxy(meth)acrylates having a weight-average molecular weight of 200 or more and less than 1,000. Commercially available polyester(meth)acrylates include those manufactured by Arakawa Chemical Industries Co., Ltd. under the trade name of the Beamset 700 series, such as Beamset 700 (hexafunctional), Beamset 710 (tetrafunctional), and Beamset 720 (trifunctional). Epoxy(meth)acrylates include those manufactured by Showa Polymer Co., Ltd. under the trade name of the SP series, such as SP-1506, 500, SP-1507, and 480, and those manufactured by VR series, such as VR-77; and those manufactured by Shin-Nakamura Chemical Co., Ltd. under the trade names of EA-1010 / ECA, EA-11020, EA-1025, and EA-6310 / ECA.

[0294] The curable composition for forming an HC layer according to the second aspect (2), which is a preferred embodiment of the second aspect, includes b) a radically polymerizable compound containing three or more ethylenically unsaturated groups per molecule. Hereinafter, the b) compound containing three or more ethylenically unsaturated groups per molecule will also be referred to as "component b" (hereinafter). Examples of component b) include esters of polyhydric alcohols and (meth)acrylic acid, vinylbenzene and its derivatives, vinyl sulfone, and (meth)acrylamide. Among these, radically polymerizable compounds containing three or more radically polymerizable groups selected from the group consisting of acryloyl groups and methacryloyl groups per molecule are preferred. Specific examples include esters of polyhydric alcohols and (meth)acrylic acid, which contain three or more ethylenically unsaturated groups per molecule. More specifically, for example, (di)pentaerythritol tetra(meth)acrylate, (di)pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, EO-modified trimethylolpropane tri(meth)acrylate, PO-modified trimethylolpropane tri(meth)acrylate, EO-modified phosphate tri(meth)acrylate, trimethylolethane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, (di)pentaerythritol Examples of the (di)pentaerythritol include tris(acryloxyethyl)isocyanurate, tripentaerythritol triacrylate, tripentaerythritol hexa(meth)acrylate, 1,2,3-cyclohexane tetramethacrylate, polyurethane polyacrylate, polyester polyacrylate, caprolactone-modified tris(acryloxyethyl)isocyanurate, tripentaerythritol triacrylate, tripentaerythritol hexatriacrylate, 1,2,4-cyclohexane tetra(meth)acrylate, and pentaglycerol triacrylate. The term "(di)pentaerythritol" used above refers to either or both of pentaerythritol and dipentaerythritol.

[0295] Furthermore, a resin containing three or more radical polymerizable groups selected from the group consisting of acryloyl groups and methacryloyl groups in one molecule is also preferred. Examples of the resin containing three or more radical polymerizable groups selected from the group consisting of acryloyl groups and methacryloyl groups in one molecule include polyester resins, polyether resins, acrylic resins, epoxy resins, urethane resins, alkyd resins, spiroacetal resins, polybutadiene resins, polythiolpolyene resins, and polymers of polyfunctional compounds such as polyhydric alcohols.

[0296] Examples of radically polymerizable compounds containing three or more radically polymerizable groups selected from the group consisting of acryloyl groups and methacryloyl groups in one molecule include the exemplified compounds shown in paragraph 0096 of JP-A-2007-256844. Furthermore, examples of radically polymerizable compounds containing three or more radically polymerizable groups selected from the group consisting of acryloyl groups and methacryloyl groups in one molecule include esters of polyols and (meth)acrylic acid, such as KAYARADDPHA, DPHA-2C, PET-30, TMPTA, TPA-320, TPA-330, RP-1040, T-1420, D-310, DPCA-20, DPCA-30, DPCA-60, and GPO-303 manufactured by Nippon Kayaku Co., Ltd., and V#400 and V#36095D manufactured by Osaka Organic Chemical Industry Co., Ltd. In addition, Shiko UV-1400B, UV-1700B, UV-6300B, UV-7550B, UV-7600B, UV-7605B, UV-7610B, UV- 7620EA, UV-7630B, UV-7640B, UV-6630B, UV-7000B, UV-7510B, UV-7461TE, UV-3000B, UV-3200B, UV-3210EA, UV-3310EA, UV-3310B, UV-3500BA, UV-3520TL, UV-3700B, UV-6100B, UV-6640B, UV-2000B, UV-2010B, UV-2250EA, UV-2750B (manufactured by Nippon Synthetic Chemical Industry Co., Ltd.), UL-503LN (manufactured by Kyoeisha Chemical Co., Ltd.), Unidic 17-806, Unidic 17-813, Unidic V-4030, Unidic V-4000BA (manufactured by Dainippon Ink & Chemicals, Inc.), EB-1290K, EB-220, EB-5129, EB-1830, EB-4358 (manufactured by Daicel UCB), Hicorp AU-2010, Hicorp AU-2020 (manufactured by TOKUSHIKI Co., Ltd.), Aronix M-1960 (manufactured by Toagosei Co., Ltd.), Other suitable compounds that can be used include tri- or higher functional urethane acrylate compounds such as Artresin UN-3320HA, UN-3320HC, UN-3320HS, UN-904, and HDP-4T, and tri- or higher functional polyester compounds such as Aronix M-8100, M-8030, and M-9050 (manufactured by Toagosei) and KBM-8307 (manufactured by Daicel Cytec).As component b), only one type may be used, or two or more types having different structures may be used in combination.

[0297] As described above, the HC layer obtained by curing the curable composition for forming an HC layer of the second aspect (2) can preferably contain 15 to 70 mass% of the structure derived from a) above, 25 to 80 mass% of the structure derived from b) above, 0.1 to 10 mass% of c) above, and 0.1 to 10 mass% of d) above, when the total solid content of the HC layer is taken as 100 mass%. The structure derived from b) is preferably contained in an amount of 40 to 75 mass%, more preferably 60 to 75 mass%, when the total solid content of the HC layer is taken as 100 mass%. Furthermore, the curable composition for forming an HC layer of the second aspect (2) preferably contains 40 to 75 mass%, more preferably 60 to 75 mass%, of component b) when the total solid content of the curable composition for forming an HC layer is taken as 100 mass%.

[0298] -Cationically Polymerizable Compound- The curable composition for forming an HC layer according to the second embodiment preferably contains at least one radically polymerizable compound and at least one cationically polymerizable compound. Any cationically polymerizable compound having a polymerizable group capable of cation polymerization (cationically polymerizable group) can be used without any limitations. Furthermore, the number of cationically polymerizable groups contained in one molecule is at least one. The cationically polymerizable compound may be a monofunctional compound containing one cationically polymerizable group per molecule, or a polyfunctional compound containing two or more cationically polymerizable groups per molecule. The number of cationically polymerizable groups contained in the polyfunctional compound is not particularly limited, but may be, for example, 2 to 6 per molecule. Furthermore, the two or more cationically polymerizable groups contained in one molecule of the polyfunctional compound may be the same, or may be two or more different in structure.

[0299] In one embodiment, the cationically polymerizable compound preferably has one or more radically polymerizable groups in one molecule in addition to the cationically polymerizable group. For the radically polymerizable group possessed by such a cationically polymerizable compound, the above description of the radically polymerizable compound can be referred to. The radically polymerizable group is preferably an ethylenically unsaturated group, and the ethylenically unsaturated group is more preferably a radically polymerizable group selected from the group consisting of a vinyl group, an acryloyl group, and a methacryloyl group. The number of radically polymerizable groups in one molecule of the cationically polymerizable compound having a radically polymerizable group is at least one, preferably one to three, and more preferably one.

[0300] The cationically polymerizable group is preferably an oxygen-containing heterocyclic group or a vinyl ether group. The cationically polymerizable compound may contain one or more oxygen-containing heterocyclic groups and one or more vinyl ether groups in one molecule.

[0301] The oxygen-containing heterocycle may be a monocycle or a fused ring. Those having a bicyclo skeleton are also preferred. The oxygen-containing heterocycle may be a non-aromatic ring or an aromatic ring, and a non-aromatic ring is preferred. Specific examples of monocycles include an epoxy ring, a tetrahydrofuran ring, and an oxetane ring. Those having a bicyclo skeleton include an oxabicyclo ring. The cationically polymerizable group containing an oxygen-containing heterocycle is contained in the cationically polymerizable compound as a monovalent substituent or as a divalent or higher polyvalent substituent. The fused ring may be one in which two or more oxygen-containing heterocycles are fused, or one or more oxygen-containing heterocycles are fused with one or more ring structures other than the oxygen-containing heterocycle. Examples of ring structures other than the oxygen-containing heterocycle include, but are not limited to, cycloalkane rings such as a cyclohexane ring.

[0302] Specific examples of oxygen-containing heterocycles are shown below, but the present invention is not limited to these examples.

[0303]

[0304] The cationically polymerizable compound may contain a partial structure other than the cationically polymerizable group. Such a partial structure is not particularly limited and may be a linear structure, a branched structure, or a cyclic structure. These partial structures may contain one or more heteroatoms such as oxygen atoms or nitrogen atoms.

[0305] A preferred embodiment of the cationically polymerizable compound is a compound containing a cyclic structure as the cationically polymerizable group or as a partial structure other than the cationically polymerizable group (cyclic structure-containing compound). The cyclic structure contained in the cyclic structure-containing compound may be, for example, one or may be two or more cyclic structures per molecule. The number of cyclic structures contained in the cyclic structure-containing compound is, for example, 1 to 5 per molecule, but is not particularly limited. A compound containing two or more cyclic structures per molecule may contain the same cyclic structure, or may contain two or more cyclic structures with different structures.

[0306] An example of the cyclic structure contained in the cyclic structure-containing compound is an oxygen-containing heterocycle, the details of which are as described above.

[0307] The cationic polymerizable group equivalent (= B / C), calculated by dividing the molecular weight (hereinafter referred to as "B") by the number of cationic polymerizable groups (hereinafter referred to as "C") contained in one molecule of the cationic polymerizable compound, is, for example, 300 or less. From the viewpoint of improving adhesion between the HC layer obtained by curing the curable composition for forming an HC layer and the resin film, it is preferably less than 150. On the other hand, from the viewpoint of the hygroscopicity of the HC layer obtained by curing the curable composition for forming an HC layer, it is preferable that the cationic polymerizable group equivalent is 50 or more. In one embodiment, the cationic polymerizable group contained in the cationic polymerizable compound for which the cationic polymerizable group equivalent is calculated can be an epoxy group (epoxy ring). That is, in one embodiment, the cationic polymerizable compound is an epoxy ring-containing compound. From the viewpoint of improving adhesion between the HC layer obtained by curing the curable composition for forming an HC layer and the resin film, it is preferable that the epoxy group equivalent, calculated by dividing the molecular weight by the number of epoxy rings contained in one molecule of the epoxy ring-containing compound, is less than 150. The epoxy group equivalent of the epoxy ring-containing compound is, for example, 50 or more.

[0308] The molecular weight of the cationically polymerizable compound is preferably not more than 500, and more preferably not more than 300. A cationically polymerizable compound having a molecular weight within the above range tends to easily penetrate into the transparent substrate described below, and is presumed to be able to contribute to improving the adhesion between the HC layer obtained by curing the HC layer-forming curable composition and the transparent resin substrate.

[0309] The curable composition for forming an HC layer of the second aspect (2) includes a) a cationically polymerizable compound containing an alicyclic epoxy group and an ethylenically unsaturated group, wherein the number of the alicyclic epoxy group contained in one molecule and the number of the ethylenically unsaturated group contained in one molecule are one, and the molecular weight is 300 or less. Hereinafter, the above a) will be referred to as "component a)."

[0310] Examples of the ethylenically unsaturated group include radical polymerizable groups containing an acryloyl group, a methacryloyl group, a vinyl group, a styryl group, or an allyl group, and particularly, an acryloyl group, a methacryloyl group, or a C(O)OCH═CH 2The number of alicyclic epoxy groups and ethylenically unsaturated groups in one molecule is preferably one each, and more preferably an acryloyl group or a methacryloyl group.

[0311] The molecular weight of component a) is 300 or less, preferably 210 or less, and more preferably 200 or less.

[0312] A preferred embodiment of component a) is a compound represented by the following general formula (1).

[0313]

[0314] In general formula (1), R represents a monocyclic hydrocarbon or a crosslinked hydrocarbon, L represents a single bond or a divalent linking group, and Q represents an ethylenically unsaturated group.

[0315] When R in general formula (1) is a monocyclic hydrocarbon, the monocyclic hydrocarbon is preferably an alicyclic hydrocarbon, more preferably an alicyclic group having 4 to 10 carbon atoms, even more preferably an alicyclic group having 5 to 7 carbon atoms, and particularly preferably an alicyclic group having 6 carbon atoms. Of these, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, or a cycloheptyl group is preferred, and a cyclohexyl group is more preferred.

[0316] When R in general formula (1) is a bridged hydrocarbon, the bridged hydrocarbon is preferably a bicyclic bridged hydrocarbon (bicyclo ring) or a tricyclic bridged hydrocarbon (tricyclo ring). Specific examples include bridged hydrocarbons having 5 to 20 carbon atoms, such as norbornyl, bornyl, isobornyl, tricyclodecyl, dicyclopentenyl, dicyclopentanyl, tricyclopentenyl, tricyclopentanyl, adamantyl, and adamantyl groups substituted with a lower (e.g., 1 to 6 carbon atoms) alkyl group.

[0317] When L represents a divalent linking group, the divalent linking group is preferably a divalent aliphatic hydrocarbon group. The number of carbon atoms in the divalent aliphatic hydrocarbon group is preferably 1 to 6, more preferably 1 to 3, and even more preferably 1. The divalent aliphatic hydrocarbon group is preferably a linear, branched, or cyclic alkylene group, more preferably a linear or branched alkylene group, and even more preferably a linear alkylene group.

[0318] Q is an ethylenically unsaturated group including an acryloyl group, a methacryloyl group, a vinyl group, a styryl group, or an allyl group, and is preferably an acryloyl group, a methacryloyl group, or a C(O)OCH═CH 2 is preferred, and an acryloyl group or a methacryloyl group is more preferred.

[0319] Specific examples of component a) include the various compounds exemplified in paragraph 0015 of JP-A No. 10-017614, compounds represented by the following general formula (1A) or (1B), and 1,2-epoxy-4-vinylcyclohexane. Of these, compounds represented by the following general formula (1A) or (1B) are preferred. Note that isomers of the compound represented by the following general formula (1A) are also preferred.

[0320]

[0321]

[0322] In general formulas (1A) and (1B), R 1 represents a hydrogen atom or a methyl group, L 2 represents a divalent aliphatic hydrocarbon group having 1 to 6 carbon atoms.

[0323] L in general formulas (1A) and (1B) 2 The divalent aliphatic hydrocarbon group represented by the formula (I) has 1 to 6 carbon atoms, preferably 1 to 3 carbon atoms, and more preferably 1 carbon atom. As the divalent aliphatic hydrocarbon group, a linear, branched, or cyclic alkylene group is preferred, a linear or branched alkylene group is more preferred, and a linear alkylene group is even more preferred.

[0324] The HC layer obtained by curing the curable composition for forming an HC layer of the second aspect (2) preferably contains 15 to 70 mass %, more preferably 18 to 50 mass %, and even more preferably 22 to 40 mass % of the structure derived from a) above, when the total solid content of the HC layer is taken as 100 mass %. Furthermore, the curable composition for forming an HC layer of the second aspect (2) preferably contains 15 to 70 mass %, more preferably 18 to 50 mass %, and even more preferably 22 to 40 mass % of component a) when the total solid content of the curable composition for forming an HC layer is taken as 100 mass %.

[0325] Another example of the cyclic structure contained in the cyclic structure-containing compound is an alicyclic structure. Examples of the alicyclic structure include a cyclo ring, a dicyclo ring, and a tricyclo ring structure. More specifically, examples include a dicyclopentanyl ring and a cyclohexane ring.

[0326] The cationically polymerizable compounds described above can be synthesized by known methods, and are also available as commercial products.

[0327] Examples of the cationically polymerizable compound containing an oxygen-containing heterocycle as a cationically polymerizable group include 3,4-epoxycyclohexylmethyl methacrylate (commercially available products such as Cyclomer M100 manufactured by Daicel Corporation), 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexanecarboxylate (commercially available products such as UVR6105 and UVR6110 manufactured by Union Carbide and Celloxide 2021 manufactured by Daicel Chemical Industries, Ltd.), bis(3,4-epoxycyclohexylmethyl)adipate (for example, UVR6128 manufactured by Union Carbide), vinylcyclohexene monoepoxide (for example, Celloxide 2000 manufactured by Daicel Chemical Industries, Ltd.), ε-caprolactone-modified 3,4-epoxycyclohexylmethyl 3', Examples of such esters include 4'-epoxycyclohexane carboxylate (e.g., Celloxide 2081 manufactured by Daicel Chemical Industries, Ltd.), 1-methyl-4-(2-methyloxiranyl)-7-oxabicyclo[4,1,0]heptane (e.g., Celloxide 3000 manufactured by Daicel Chemical Industries, Ltd.), 7,7'-dioxa-3,3'-bis[bicyclo[4.1.0]heptane] (e.g., Celloxide 8000 manufactured by Daicel Chemical Industries, Ltd.), 3-ethyl-3-hydroxymethyloxetane, 1,4-bis{[(3-ethyl-3-oxetanyl)methoxy]methyl}benzene, 3-ethyl-3-(phenoxymethyl)oxetane, 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane, and di[1-ethyl(3-oxetanyl)]methyl ether.

[0328] Furthermore, examples of cationically polymerizable compounds containing a vinyl ether group as the cationically polymerizable group include 1,4-butanediol divinyl ether, 1,6-hexanediol divinyl ether, nonanediol divinyl ether, cyclohexanediol divinyl ether, cyclohexanedimethanol divinyl ether, triethylene glycol divinyl ether, trimethylolpropane trivinyl ether, and pentaerythritol tetravinyl ether. As the cationically polymerizable compound containing a vinyl ether group, those having an alicyclic structure are also preferred.

[0329] Further, examples of the cationically polymerizable compound include compounds exemplified in JP-A-8-143806, JP-A-8-283320, JP-A-2000-186079, JP-A-2000-327672, JP-A-2004-315778, and JP-A-2005-29632.

[0330] Specific examples of the cationically polymerizable compound include compounds B-1 to B-14, but the present invention is not limited to these examples.

[0331]

[0332]

[0333]

[0334] Furthermore, from the viewpoint of improving adhesion between the HC layer obtained by curing the curable composition for forming an HC layer and the resin film, the following aspects can be mentioned as preferred aspects of the curable composition for forming an HC layer. It is more preferable that one or more of the following aspects are satisfied, and even more preferable that two or more are satisfied. It is also preferable that one cationically polymerizable compound satisfies multiple aspects. (1) The cationically polymerizable compound includes a cationically polymerizable compound having a cationically polymerizable group equivalent of less than 150. Preferably, the cationically polymerizable compound includes an epoxy group-containing compound having an epoxy group equivalent of less than 150. (2) The cationically polymerizable compound includes an ethylenically unsaturated group.

[0335] The content of the cationically polymerizable compound in the curable composition for forming an HC layer is preferably 10 parts by mass or more, more preferably 15 parts by mass or more, and even more preferably 20 parts by mass or more, per 100 parts by mass of the total content of the radically polymerizable compound and the cationically polymerizable compound. The content of the cationically polymerizable compound in the curable composition for forming an HC layer is preferably 50 parts by mass or less, per 100 parts by mass of the total content of the radically polymerizable compound and the cationically polymerizable compound. The content of the cationically polymerizable compound in the curable composition for forming an HC layer is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, and even more preferably 1 part by mass or more, per 100 parts by mass of the total content of the first radically polymerizable compound and the cationically polymerizable compound. Meanwhile, the content of the cationically polymerizable compound is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, per 100 parts by mass of the total content of the first radically polymerizable compound and the cationically polymerizable compound. In this specification, a compound having both a cationically polymerizable group and a radically polymerizable group is classified as a cationically polymerizable compound, and the content thereof in the curable composition for forming the HC layer is specified.

[0336] -Polymerization initiator- The curable composition for forming an HC layer preferably contains a polymerization initiator, and more preferably contains a photopolymerization initiator. The curable composition for forming an HC layer containing a radical polymerizable compound preferably contains a radical photopolymerization initiator, and the curable composition for forming an HC layer containing a cationic polymerizable compound preferably contains a cationic photopolymerization initiator. Only one type of radical photopolymerization initiator may be used, or two or more types with different structures may be used in combination. This also applies to cationic photopolymerization initiators. Each photopolymerization initiator will be explained in turn below.

[0337] (i) Radical Photopolymerization Initiator The radical photopolymerization initiator may be any one that can generate radicals as active species upon irradiation with light, and known radical photopolymerization initiators can be used without any limitations. Specific examples include diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, benzyl dimethyl ketal, 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-2-morpholino(4-thiomethylphenyl)propan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, 2-hydroxy-2-methyl-1-[4-( acetophenones such as 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one; oxime esters such as 1,2-octanedione, 1-[4-(phenylthio)-, 2-(O-benzoyloxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime); Benzoins such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether; benzophenone, methyl ortho-benzoylbenzoate, 4-phenylbenzophenone, 4-benzoyl-4'-methyl-diphenyl sulfide, 3,3',4,4'-tetra(t-butylperoxycarbonyl)benzophenone, 2,4,6-trimethylbenzophenone, 4-benzoyl-N,N-dimethyl-N-[2-(1-oxo-1,2-dimethylphenyl)benzoyl] ... benzophenones such as (4-benzoylbenzyl)trimethylammonium chloride, (4-benzoylbenzyl)trimethylammonium bromide, and (4-benzoylbenzyl)trimethylammonium chloride; thioxanthones such as 2-isopropylthioxanthone, 4-isopropylthioxanthone, 2,4-diethylthioxanthone, 2,4-dichlorothioxanthone, 1-chloro-4-propoxythioxanthone, and 2-(3-dimethylamino-2-hydroxy)-3,4-dimethyl-9H-thioxanthone-9-one mesochloride;Examples of the photopolymerization initiator include acylphosphine oxides such as 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide, and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide. Furthermore, examples of the photopolymerization initiator aids that may be used in combination include triethanolamine, triisopropanolamine, 4,4'-dimethylaminobenzophenone (Michler's ketone), 4,4'-diethylaminobenzophenone, 2-dimethylaminoethylbenzoic acid, ethyl 4-dimethylaminobenzoate, (n-butoxy)ethyl 4-dimethylaminobenzoate, isoamyl 4-dimethylaminobenzoate, 2-ethylhexyl 4-dimethylaminobenzoate, 2,4-diethylthioxanthone, and 2,4-diisopropylthioxanthone. The above radical photopolymerization initiators and auxiliaries can be synthesized by known methods and are also available as commercial products. Preferred examples of commercially available radical photopolymerization initiators include Irgacure (127, 651, 184, 819, 907, 1870 (CGI-403 / Irg184=7 / 3 mixed initiator, 500, 369, 1173, 2959, 4265, 4263, etc.), OXE01) manufactured by BASF, KAYACURE (DETX-S, BP-100, BDMK, CTX, BMS, 2-EAQ, ABQ, CPTX, EPD, ITX, QTX, BTC, MCA, etc.) manufactured by Nippon Kayaku, and Esacure (KIP100F, KB1, EB3, BP, X33, KT046, KT37, KIP150, TZT) manufactured by Sartomer;

[0338] The content of the radical photopolymerization initiator in the curable composition for forming an HC layer is not particularly limited, and may be appropriately adjusted within a range in which the polymerization reaction (radical polymerization) of the radical polymerizable compound proceeds satisfactorily. The content is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 1 to 10 parts by mass, relative to 100 parts by mass of the radical polymerizable compound contained in the curable composition for forming an HC layer.

[0339] (ii) Cationic Photopolymerization Initiator The cationic photopolymerization initiator may be any one capable of generating cations as active species upon irradiation with light, and known cationic photopolymerization initiators can be used without any limitations. Specific examples include known sulfonium salts, ammonium salts, iodonium salts (e.g., diaryliodonium salts), triarylsulfonium salts, diazonium salts, and iminium salts. More specific examples include cationic photopolymerization initiators represented by formulas (25) to (28) shown in paragraphs

[0050] to

[0053] of JP-A-8-143806, and those exemplified as cationic polymerization catalysts in paragraph

[0020] of JP-A-8-283320. Cationic photopolymerization initiators can be synthesized by known methods and are also commercially available. Examples of commercially available products that can be used include CI-1370, CI-2064, CI-2397, CI-2624, CI-2639, CI-2734, CI-2758, CI-2823, CI-2855, and CI-5102 manufactured by Nippon Soda; PHOTOINITIATOR 2047 manufactured by Rhodia; UVI-6974 and UVI-6990 manufactured by Union Carbide; and CPI-10P manufactured by San-Apro.

[0340] As the cationic photopolymerization initiator, a diazonium salt, an iodonium salt, a sulfonium salt, or an iminium salt is preferred from the viewpoint of the sensitivity of the photopolymerization initiator to light, the stability of the compound, etc. Furthermore, an iodonium salt is more preferred from the viewpoint of weather resistance.

[0341] Specific examples of commercially available iodonium salt-based cationic photopolymerization initiators include B2380 manufactured by Tokyo Chemical Industry Co., Ltd., BBI-102 manufactured by Midori Chemical Industry Co., Ltd., WPI-113 manufactured by Wako Pure Chemical Industries, Ltd., WPI-124 manufactured by Wako Pure Chemical Industries, Ltd., WPI-169 manufactured by Wako Pure Chemical Industries, Ltd., WPI-170 manufactured by Wako Pure Chemical Industries, Ltd., and DTBPI-PFBS manufactured by Toyo Synthetic Chemical Industry Co., Ltd.

[0342] Specific examples of iodonium salt compounds that can be used as cationic photopolymerization initiators include the following compounds PAG-1 and PAG-2.

[0343]

[0344]

[0345] The content of the cationic photopolymerization initiator in the curable composition for forming an HC layer is not particularly limited, and may be appropriately adjusted within a range in which the polymerization reaction (cationic polymerization) of the cationically polymerizable compound proceeds well. The content of the cationic photopolymerization initiator in the curable composition for forming an HC layer is preferably 0.1 to 200 parts by mass, more preferably 1 to 150 parts by mass, and even more preferably 2 to 100 parts by mass, relative to 100 parts by mass of the cationically polymerizable compound.

[0346] Other photopolymerization initiators include those described in paragraphs 0052 to 0055 of JP-A-2009-204725, the contents of which are incorporated herein by reference.

[0347] -Components that may be optionally contained in the curable composition for forming an HC layer- The curable composition for forming an HC layer contains at least one component that has the property of being cured by irradiation with active energy rays and a compound selected from the group consisting of polysiloxane-containing compounds and fluorine-containing compounds, and may optionally contain, and preferably contains, at least one polymerization initiator. Details of these are as described above. Next, various components that may optionally be contained in the curable composition for forming an HC layer will be described.

[0348] (i) Inorganic Particles The HC layer-forming curable composition may contain inorganic particles having an average primary particle size of less than 2 μm. From the viewpoint of improving the hardness of the HC layer obtained by curing the HC layer-forming curable composition (and further improving the hardness of a liquid crystal panel having this front panel), the HC layer-forming curable composition and the HC layer obtained by curing this composition preferably contain inorganic particles having an average primary particle size of less than 2 μm. The average primary particle size of the inorganic particles is preferably 10 nm to 1 μm, more preferably 10 nm to 100 nm, and even more preferably 10 nm to 50 nm. The average primary particle size of the inorganic particles and the matte particles described below is determined by observing the particles with a transmission electron microscope (magnification 500,000 to 2,000,000 times), observing 100 randomly selected particles (primary particles), and averaging the particle sizes of these particles to determine the average primary particle size.

[0349] Examples of the inorganic particles include silica particles, titanium dioxide particles, zirconium oxide particles, and aluminum oxide particles, with silica particles being preferred.

[0350] The inorganic particles are preferably surface-treated with a surface modifier containing an organic segment to enhance their affinity with the organic components contained in the curable composition for forming an HC layer. Surface modifiers preferably contain, in the same molecule, a functional group capable of bonding with or adsorbing to the inorganic particles and a functional group having high affinity with the organic component. Surface modifiers having functional groups capable of bonding with or adsorbing to the inorganic particles include silane-based surface modifiers, metal alkoxide surface modifiers such as aluminum, titanium, and zirconium, and surface modifiers having anionic groups such as phosphate groups, sulfate groups, sulfonate groups, and carboxylate groups. Functional groups with high affinity with the organic component include functional groups having similar hydrophilicity to the organic component and functional groups capable of chemically bonding with the organic component. Among these, functional groups capable of chemically bonding with the organic component are preferred, with ethylenically unsaturated groups or ring-opening polymerizable groups being more preferred.

[0351] Preferred inorganic particle surface modifiers are metal alkoxide surface modifiers or polymerizable compounds having an anionic group and an ethylenically unsaturated group or a ring-opening polymerizable group in the same molecule. These surface modifiers chemically bond the inorganic particles and the organic component, thereby increasing the crosslink density of the HC layer and, as a result, improving scratch resistance.

[0352] Specific examples of the surface modifier include the following exemplary compounds S-1 to S-8: S-1H 2 C=C(X)COOC 3 H 6 Si(OCH 3 ) 3 S-2H 2 C=C(X)COOC 2 H 4 OTi (OC 2 H 5 ) 3 S-3H 2 C=C(X)COOC 2 H 4 OCOC5 H 10 OPO (OH) 2 S-4 (H 2 C=C(X)COOC 2 H 4 OCOC 5 H 10 O) 2 POOH S-5H 2 C=C(X)COOC 2 H 4 OSO 3 H S-6H 2 C=C(X)COO(C 5 H 10 COO) 2 H S-7H 2 C=C(X)COOC 5 H 10 COOH S-8CH 2 CH(O)CH 2 O.C. 3 H 6 Si(OCH 3 ) 3 (X represents a hydrogen atom or a methyl group)

[0353] The surface modification of inorganic particles with a surface modifier is preferably carried out in a solution. When the inorganic particles are mechanically dispersed, the surface modifier may be present together, or the inorganic particles may be mechanically dispersed and then the surface modifier added and stirred, or the inorganic particles may be surface-modified before being mechanically dispersed (if necessary, heated, dried, then heated, or pH (power hydrogen) changed), and then dispersed. A highly polar organic solvent is preferred as the solvent for dissolving the surface modifier. Specific examples include known solvents such as alcohols, ketones, and esters.

[0354] The content of inorganic particles is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, when the total solid content of the curable composition for forming an HC layer is taken as 100% by mass. The lower limit of the content is not particularly limited and may be 0% by mass (no inorganic particles may be contained in the HC layer), but if inorganic particles are contained, it is preferably 1% by mass or more, more preferably 7% by mass or more. The shape of the primary particles of the inorganic particles may be either spherical or non-spherical, and the primary particles of the inorganic particles are preferably spherical. From the viewpoint of further improving hardness, it is more preferable that the primary particles of the inorganic particles are present in the HC layer obtained by curing the curable composition for forming an HC layer as higher-order particles of non-spherical secondary particles or higher, in which 2 to 10 spherical inorganic particles (primary particles) are linked together.

[0355] Specific examples of inorganic particles include ELCOMV-8802 (spherical silica particles having an average primary particle size of 15 nm, manufactured by JGC Catalysts and Chemicals), ELCOMV-8803 (irregular shaped silica particles, manufactured by JGC Catalysts and Chemicals), MiBK-SD (spherical silica particles having an average primary particle size of 10 to 20 nm, manufactured by Nissan Chemical Industries, Ltd.), MEK-AC-2140Z (spherical silica particles having an average primary particle size of 10 to 20 nm, manufactured by Nissan Chemical Industries, Ltd.), MEK-AC-4130 (spherical silica particles having an average primary particle size of 45 nm, manufactured by Nissan Chemical Industries, Ltd.), MiBK-SD-L (spherical silica particles having an average primary particle size of 40 to 50 nm, manufactured by Nissan Chemical Industries, Ltd.), MEK-AC-5140Z (spherical silica particles having an average primary particle size of 85 nm, manufactured by Nissan Chemical Industries, Ltd.), and RX-300 (spherical silica particles having an average primary particle size of 7 nm, manufactured by Nippon Aerosil Co., Ltd.). Among these, MEK-AC-2140Z manufactured by Nissan Chemical Industries, Ltd. is preferred from the viewpoint of further improving hardness.

[0356] (ii) Matte Particles The curable composition for forming an HC layer may also contain matte particles. Matte particles refer to particles having an average primary particle size of 2 μm or more, and may be inorganic particles, organic particles, or particles of an inorganic-organic composite material. The shape of the matte particles may be spherical or non-spherical. The average primary particle size of the matte particles is preferably 2 to 20 μm, more preferably 4 to 14 μm, and even more preferably 6 to 10 μm.

[0357] Examples of matte particles include silica particles and TiO 2 and organic particles such as crosslinked acrylic particles, crosslinked acrylic-styrene particles, crosslinked styrene particles, melamine resin particles, and benzoguanamine resin particles. Among these, organic particles are preferred as matte particles, and crosslinked acrylic particles, crosslinked acrylic-styrene particles, or crosslinked styrene particles are more preferred.

[0358] The matte particles are contained in an amount of 0.10 g / cm 3 per unit volume in the HC layer obtained by curing the curable composition for forming the HC layer. 3 More than this is preferred, and 0.10 to 0.40 g / cm 3 More preferably, 0.10 to 0.30 g / cm 3 is more preferred.

[0359] (iii) Ultraviolet Absorber (UV Absorber) The curable composition for forming the HC layer preferably contains an ultraviolet absorber. Examples of ultraviolet absorbers include benzotriazole compounds and triazine compounds. Here, the benzotriazole compound is a compound having a benzotriazole ring. Specific examples include the various benzotriazole-based ultraviolet absorbers described in paragraph 0033 of JP-A-2013-111835. The triazine compound is a compound having a triazine ring. Specific examples include the various triazine-based ultraviolet absorbers described in paragraph 0033 of JP-A-2013-111835. The content of the ultraviolet absorber in the HC layer is not particularly limited, and is preferably, for example, 0.1 to 10 parts by mass per 100 parts by mass of the resin contained in the HC layer. For more information on ultraviolet absorbers, see paragraph 0032 of JP-A-2013-111835. In this specification, ultraviolet light refers to light having a central emission wavelength in the wavelength band of 200 to 380 nm.

[0360] (iv) Leveling agent The curable composition for forming HC layer preferably contains a leveling agent. As the leveling agent, a fluorine-containing polymer is preferably used. For example, the fluoroaliphatic group-containing polymer described in Japanese Patent No. 5175831 can be mentioned. In addition, a fluoroaliphatic group-containing polymer in which the content of the fluoroaliphatic group-containing monomer represented by general formula (1) constituting the fluoroaliphatic group-containing polymer is 50 mass% or less of the total polymerized units can also be used as a leveling agent. In addition, the leveling agent described in (vi) other components described below can also be contained in addition to the above.

[0361] When the HC layer-forming curable composition contains a leveling agent, the content of the leveling agent is preferably 0.01 to 7 mass%, more preferably 0.05 to 5 mass%, and even more preferably 0.1 to 2 mass%, based on the solid content of the HC layer-forming curable composition. The HC layer-forming curable composition may contain only one type of leveling agent, or may contain two or more types. When two or more types are contained, the total amount thereof is preferably in the above range.

[0362] (v) Solvent The curable composition for forming an HC layer preferably contains a solvent. The solvent is preferably an organic solvent, and one or more organic solvents can be mixed in any ratio and used. Examples of organic solvents include alcohols such as methanol, ethanol, propanol, n-butanol, and i-butanol; ketones such as acetone, methyl isobutyl ketone, methyl ethyl ketone, and cyclohexanone; cellosolves such as ethyl cellosolve; aromatics such as toluene and xylene; glycol ethers such as propylene glycol monomethyl ether; acetate esters such as methyl acetate, ethyl acetate, and butyl acetate; and diacetone alcohol. Among these, it is preferable to use a solvent selected from cyclohexanone, methyl ethyl ketone, methyl isobutyl ketone, butyl acetate, isopropyl acetate, and methyl acetate mixed in any ratio.

[0363] The amount of solvent in the HC layer-forming curable composition can be adjusted as appropriate within a range that ensures the coating suitability of the composition. For example, the solvent content is preferably 50 to 500 parts by mass, more preferably 80 to 200 parts by mass, relative to 100 parts by mass of the total amount of the polymerizable compound and the photopolymerization initiator. Furthermore, the solid content of the HC-forming curable composition is preferably 10 to 90% by mass, more preferably 50 to 80% by mass, and even more preferably 65 to 75% by mass, relative to the total mass of the HC-forming curable composition.

[0364] (vi) Other Components In addition to the above components, the curable composition for forming an HC layer can contain any amount of one or more known additives. Examples of additives include surface conditioners, leveling agents, polymerization inhibitors, and polyrotaxanes. For details, see, for example, paragraphs 0032 to 0034 of JP 2012-229412 A. However, the additives are not limited to these, and various additives that can generally be added to curable compositions for forming an HC layer can be used.

[0365] The curable composition for forming the HC layer can be prepared by mixing the above-described various components simultaneously or sequentially in any order. The preparation method is not particularly limited, and a known mixer or the like can be used for preparation.

[0366] -Thickness of HC Layer- The thickness of the HC layer is preferably 1 to 100 μm, more preferably 1 to 20 μm, and even more preferably 3 to 20 μm.

[0367] The thickness of the HC layer is measured by cutting the HC layer with a microtome to cut out a cross section, staining it overnight with an approximately 3% by mass aqueous solution of osmium tetroxide, then cutting out the surface again and observing the cross section using a SEM (Scanning Electron Microscope).

[0368] -Method of Forming HC Layer- The method of forming the HC layer is not particularly limited, and for example, the HC layer can be formed by applying a curable composition for forming an HC layer and irradiating it with active energy rays. The application can be carried out by a known application method such as dip coating, air knife coating, curtain coating, roller coating, die coating, wire bar coating, or gravure coating. The HC layer can also be formed as an HC layer having a laminate structure of two or more layers (for example, about two to five layers) by simultaneously or sequentially applying two or more compositions having different compositions.

[0369] The HC layer can be formed by irradiating the applied HC layer-forming curable composition with active energy rays. For example, when the HC layer-forming curable composition contains a radical polymerizable compound, a cationic polymerizable compound, a radical photopolymerization initiator, and a cationic photopolymerization initiator, the polymerization reactions of the radical polymerizable compound and the cationic polymerizable compound can be initiated and progressed by the action of the radical photopolymerization initiator and the cationic photopolymerization initiator, respectively. The wavelength of the irradiated light may be determined depending on the type of polymerizable compound and polymerization initiator used. Examples of light sources for light irradiation include high-pressure mercury lamps, ultra-high-pressure mercury lamps, carbon arc lamps, metal halide lamps, xenon lamps, chemical lamps, electrodeless discharge lamps, and LEDs (light-emitting diodes), all of which emit light in the 150 to 450 nm wavelength band. The light irradiation dose is typically 30 to 3,000 mJ / cm. 2 and preferably 100 to 1500 mJ / cm 2 If necessary, a drying treatment may be carried out either before or after light irradiation, or both. The drying treatment can be carried out by blowing hot air, placing in a heating furnace, transporting in the heating furnace, or the like. When the curable composition for forming an HC layer contains a solvent, the heating temperature is not particularly limited as long as it is set to a temperature at which the solvent can be dried and removed. Here, the heating temperature refers to the temperature of the hot air or the atmospheric temperature in the heating furnace.

[0370] <Polarization conversion layer> The polarization conversion layer is a layer in which the helical orientation structure of a liquid crystal compound is fixed, and it is preferable that the pitch number x of the helical orientation structure and the film thickness y (unit: μm) of the polarization conversion layer satisfy all of the following relational expressions (a) to (c): 0.1≦x≦1.0 (a) 0.5≦y≦3.0 (b) 3000≦(1560×y) / x≦50000 (c) Note that one pitch of the helical structure of the liquid crystal compound corresponds to one turn of the helix of the liquid crystal compound. In other words, a pitch number of 1 is defined as a state in which the director of the helically oriented liquid crystal compound (the long axis direction in the case of rod-shaped liquid crystal) has rotated 360°.

[0371] When the polarization conversion layer has a helical structure of a liquid crystal compound, it can exhibit optical rotation and birefringence for visible light, which has a wavelength shorter than the reflection peak wavelength in the infrared region. Therefore, it is possible to control polarization in the visible region. By setting the pitch number x of the helical orientation structure of the polarization conversion layer and the film thickness y of the polarization conversion layer within the above-mentioned ranges, it is possible to impart the polarization conversion layer with the function of optically compensating for visible light or the function of converting linearly polarized light (p-polarized light) incident on the film into circularly polarized light.

[0372] The polarization conversion layer exhibits optical rotation and birefringence for visible light because the liquid crystal compound has a helical structure that satisfies the relational expressions (a) to (c). In particular, by setting the pitch P of the helical structure of the polarization conversion layer to a length corresponding to the pitch P of the cholesteric liquid crystal layer whose selective reflection center wavelength is in the long-wavelength infrared region, the polarization conversion layer exhibits high optical rotation and birefringence for short-wavelength visible light.

[0373] The relational expression (a) satisfies "0.1≦x≦1.0." When the pitch number x of the helical structure is 0.1 or more, sufficient optical rotation and birefringence are obtained. When the pitch number x of the helical structure is 1.0 or less, the optical rotation and birefringence are appropriate, and the desired elliptically polarized light is obtained.

[0374] The relational expression (b) is "0.5≦y≦3.0". When the thickness y of the polarization conversion layer is 0.5 μm or more, sufficient optical rotation and birefringence are obtained. When the thickness y of the polarization conversion layer is 3.0 μm or less, the optical rotation and birefringence are appropriate, the desired circularly polarized light is obtained, and alignment defects are less likely to occur, which is preferable for production.

[0375] The relational expression (c) is "3000≦(1560×y) / x≦50000". When "(1560×y) / x" is 3000 or more, the optical rotation is sufficient and the desired polarization can be obtained. When "(1560×y) / x" is 50000 or less, the optical rotation is sufficient and the desired polarization can be obtained.

[0376] The pitch number x of the helical structure of the polarization conversion layer is more preferably 0.1 to 0.8, the film thickness y is more preferably 0.6 μm to 2.6 μm, and "(1560×y) / x" is more preferably 5000 to 13000.

[0377] That is, it is preferable that the polarization conversion layer has a long pitch P of the helical structure and a small pitch number x. Specifically, it is preferable that the polarization conversion layer has a helical pitch P equivalent to the pitch P of a cholesteric liquid crystal layer having a selective reflection center wavelength in the long-wavelength infrared region and a small pitch number x. More specifically, it is preferable that the polarization conversion layer has a helical pitch P equivalent to the pitch P of a cholesteric liquid crystal layer having a selective reflection center wavelength of 3,000 to 10,000 nm and a small pitch number x. Such a polarization conversion layer more suitably exhibits the optical rotation and birefringence for visible light described above, because the selective reflection center wavelength corresponding to the pitch P is much longer than that of visible light.

[0378] Such a polarization conversion layer can be formed in the same manner as a known cholesteric liquid crystal layer, except that when forming the polarization conversion layer, it is necessary to adjust the liquid crystal compound to be used, the chiral agent to be used, the amount of chiral agent added, the film thickness, etc. so that the pitch number x of the helical structure and the film thickness y [μm] of the polarization conversion layer satisfy all of the relational expressions (a) to (c).

[0379] <Layer in which the helical orientation structure (helical structure) of a liquid crystal compound is fixed> A layer in which the helical orientation structure (helical structure) of a liquid crystal compound is fixed is a so-called cholesteric liquid crystal layer, meaning a layer in which a cholesteric liquid crystal phase is fixed. The cholesteric liquid crystal layer may be any layer in which the orientation of a liquid crystal compound in a cholesteric liquid crystal phase is maintained. The cholesteric liquid crystal layer may typically be a layer in which a polymerizable liquid crystal compound is oriented in a cholesteric liquid crystal phase, and then polymerized and cured by ultraviolet irradiation, heating, or the like to form a non-fluid layer, and at the same time, changed to a state in which the orientation form does not change due to an external field or external force. Note that in a cholesteric liquid crystal layer, it is sufficient that the optical properties of the cholesteric liquid crystal phase are maintained in the layer, and the liquid crystal compound in the layer may no longer exhibit liquid crystallinity. For example, the polymerizable liquid crystal compound may be polymerized by a curing reaction and no longer have liquid crystallinity.

[0380] As described above, the central wavelength λ of selective reflection by the cholesteric liquid crystal layer (selective reflection central wavelength) depends on the pitch P (= helical period) of the helical structure (helical orientation structure) in the cholesteric liquid crystal phase, and follows the relationship between the average refractive index n of the cholesteric liquid crystal layer and λ = n × P. As can be seen from this formula, the selective reflection central wavelength can be adjusted by adjusting the n value and / or the P value.

[0381] The helical pitch of the cholesteric liquid crystal phase depends on the type and concentration of the chiral agent used together with the polymerizable liquid crystal compound, and the desired pitch can be obtained by adjusting these factors. As described above, the helical pitch of the cholesteric liquid crystal layer used as the polarization conversion layer is adjusted so that the selective reflection center wavelength is in the long-wavelength infrared region. The method for forming the cholesteric liquid crystal layer as the polarization conversion layer is basically the same as the method for forming the cholesteric liquid crystal layer described above.

[0382] <Retardation Layer> The retardation layer imparts a phase difference (optical path difference) to two orthogonal polarized light components, thereby changing the state of incident polarized light.

[0383] When the retardation layer is disposed on the first glass plate 3 side facing the vehicle interior and provides optical compensation, the front retardation of the retardation layer may be set to a retardation that can provide optical compensation. In this case, the front retardation of the retardation layer at a wavelength of 550 nm is preferably 50 nm to 160 nm. Furthermore, when the direction corresponding to the vertically upward direction of the surface of the laminated glass is defined as 0°, the angle of the slow axis is preferably 10° to 50° or −50° to −10°.

[0384] In addition, when the retardation layer converts linearly polarized light into circularly polarized light, the retardation layer is preferably configured to give a front retardation of λ / 4, and may be configured to give a front retardation of 3λ / 4. The angle of the slow axis may be arranged so as to be oriented in a direction that converts incident linearly polarized light into circularly polarized light.

[0385] In this case, the retardation layer preferably has a front retardation at a wavelength of 550 nm in the range of 100 to 450 nm, more preferably 120 to 200 nm or 300 to 400 nm. The direction of the slow axis of the retardation layer is preferably determined depending on the incident direction of projection light for projecting an image when the laminated glass is used in an image display device and the sense of the helix of the cholesteric liquid crystal layer that constitutes the reflective layer.

[0386] The retardation layer is not particularly limited and can be appropriately selected according to purpose.For example, the retardation layer can be a stretched polycarbonate film, a stretched norbornene polymer film, a transparent film containing and oriented inorganic particles having birefringence such as strontium carbonate, a thin film obtained by obliquely depositing an inorganic dielectric on a support, a film in which a polymerizable liquid crystal compound is uniaxially aligned and fixed, and a film in which a liquid crystal compound is uniaxially aligned and fixed.

[0387] Among these, a film in which a polymerizable liquid crystal compound is uniaxially aligned and fixed is a suitable example of a retardation layer. For example, such a retardation layer can be formed by applying a liquid crystal composition containing a polymerizable liquid crystal compound to a transparent resin substrate, a temporary support, or the surface of an alignment layer, forming the polymerizable liquid crystal compound in the liquid crystal composition into a nematic alignment in a liquid crystal state, and then fixing the alignment by curing. In this case, the formation of the retardation layer can be performed in the same manner as the formation of the cholesteric liquid crystal layer described above, except that no chiral agent is added to the liquid crystal composition. However, during nematic alignment after application of the liquid crystal composition, the heating temperature is preferably 50 to 120°C, more preferably 60 to 100°C.

[0388] The retardation layer may be a layer obtained by applying a composition containing a polymer liquid crystal compound to the surface of a transparent resin substrate, a temporary support, an alignment layer, or the like, forming a nematic alignment in a liquid crystal state, and then fixing the alignment by cooling.

[0389] The thickness of the retardation layer is not particularly limited, but is preferably 0.2 to 300 μm, more preferably 0.5 to 150 μm, and even more preferably 1.0 to 80 μm. The thickness of the retardation layer formed from the liquid crystal composition is not particularly limited, but is preferably 0.2 to 10 μm, more preferably 0.5 to 5.0 μm, and even more preferably 0.7 to 2.0 μm.

[0390] The retardation layer has a slow axis tilted at an angle α with respect to an axis of the retardation layer in any direction. The direction of the slow axis can be set by, for example, rubbing an alignment film that is an underlying layer of the retardation layer.

[0391] [Windshield Glass] The laminated glass of the present invention described above may be included in windshield glass. Windshield glass refers to the window glass and windshield glass of vehicles such as cars and trains, airplanes, ships, motorcycles, and playground equipment. Windshield glass is preferably used as a windshield or windshield glass located in front of the vehicle in the traveling direction.

[0392] When a windshield glass is used in a vehicle, for example, the outer glass 1 and the inner glass 3 shown in Figures 1 to 6 are often curved glass. In this case, if the inner glass 3 faces the inside of the vehicle and the outer glass 1 faces the outside of the vehicle, the convex side of the inner glass 3 faces the outer glass 1, and the concave side of the outer glass 1 faces the inner glass 3.

[0393] There are no restrictions on the visible light transmittance of the windshield glass, but a higher value is preferable. The visible light transmittance of the windshield glass is preferably 70% or more, more preferably more than 70%, even more preferably 75% or more, and particularly preferably 80% or more. The above-mentioned visible light transmittance is preferably satisfied at every position of the windshield glass, and particularly preferably at positions where the light-emitting layer and the reflective layer are present. Because the laminated glass of the present invention has a high visible light transmittance, it can be configured to satisfy the above-mentioned visible light transmittance even when any of the glasses commonly used for windshield glass is used.

[0394] The windshield glass preferably reflects linearly polarized light. When the reflective layer is incorporated into the windshield glass to be used as a combiner for a head-up display, the projected image light is preferably p-polarized, i.e., linearly polarized, in order to suppress reflection on the surface of the windshield glass.

[0395] The shape of the windshield glass is not limited and is determined appropriately depending on the object to which the windshield glass is to be placed. The windshield glass may be, for example, flat or may have a three-dimensional shape with a curved surface such as a concave or convex surface. In the windshield glass shaped for the vehicle to be used, the direction that is the top during normal use and the viewing side such as the observer side, the driver side, and the interior side of the vehicle can be specified.

[0396] In the windshield glass, the reflective layer may be provided in a projected image display area (projected image reflection area) of the windshield glass. In addition, in the windshield glass, the reflective layer may be provided between the glass panes of a laminated glass windshield, or on the outer surface of the glass pane of the windshield glass.

[0397] When the reflective layer is provided on the outer surface of the glass plate of the windshield glass, the reflective layer may be provided either inside (on the incident side of the projected image) or outside the vehicle or the like.

[0398] The reflective layer may be provided on the entire surface of the windshield glass, or on a portion of the surface of the windshield glass, but is preferably provided on a portion. When the reflective layer is provided on a portion of the windshield glass, the reflective layer may be provided anywhere on the windshield glass, but is preferably provided so that the virtual image is displayed in a position that is easily visible to an observer such as a driver when used as a HUD. For example, the position where the reflective layer is provided on the windshield glass can be determined based on the relationship between the position of the driver's seat in a vehicle equipped with the HUD and the position where the projector is installed.

[0399] <Image Display System> The image display system of the present invention comprises the laminated glass of the present invention, an imager that irradiates the laminated glass with projection image light, and an irradiation device that irradiates the laminated glass with light. The image display system of the present invention can be used in various known image display systems such as HUD systems and AR (Augmented Reality) glasses. In particular, the image display system of the present invention is suitably used in HUD systems.

[0400] <Imager> The imager is a device for projecting image light onto the laminated glass of the present invention. The imager can be selected depending on the light source used and the application. Examples of imagers include fluorescent display tubes, LCD (Liquid Crystal Display) and LCOS (Liquid Crystal on Silicon) systems that use liquid crystal, DLP (Digital Light Processing) systems, and laser scanning systems, with LCDs being particularly preferred because they emit linearly polarized light.

[0401] In the LCD and LCOS systems, the light of each color is modulated and combined by an optical modulator and emitted from a projection lens.The DLP system is a display system that uses a DMD (Digital Micromirror Device), in which micromirrors equal in number to the number of pixels are arranged to draw images, and the light is emitted from a projection lens.

[0402] The scanning method involves scanning a light beam on a screen and creating a contrast using the afterimage of the eye; see, for example, Japanese Patent Application Laid-Open Nos. 7-270711 and 2013-228674. In a laser scanning method, intensity-modulated laser beams of each color (e.g., red, green, and blue) are combined into a single beam using a multiplexing optical system or a condenser lens, and the beam is scanned by an optical deflection unit to form an image on an intermediate image screen (described later). In the scanning method, the intensity modulation of the laser beams of each color (e.g., red, green, and blue) may be performed directly by changing the intensity of the light source, or may be performed using an external modulator. Examples of optical deflection units include a galvanometer mirror, a polygon mirror, a combination of a galvanometer mirror and a polygon mirror, and a microelectromechanical system (MEMS), among which MEMS is preferred. Examples of scanning methods include random scanning and raster scanning, but it is preferable to use raster scanning. In the raster scanning method, the laser light can be driven, for example, at a resonant frequency in the horizontal direction and at a sawtooth wave in the vertical direction. Since the scanning method does not require a projection lens, it is easy to miniaturize the device.

[0403] The light emitted from the imager may be linearly polarized or natural light (unpolarized), but it is preferable that the light emitted from the imager be linearly polarized. When the imager is an LCD or LCOS, or when an imager uses a laser light source, the emitted light is essentially linearly polarized. When the imager emits linearly polarized light and the emitted light contains light of multiple wavelengths (colors), it is preferable that the polarization directions (transmission axis directions) of the polarized light of the multiple light beams are the same or orthogonal to each other. It is known that some commercially available imagers have non-uniform polarization directions in the wavelength ranges of red, green, and blue light of the emitted light (see JP 2000-221449 A). Specifically, there is known an example in which the polarization direction of green light is orthogonal to the polarization directions of red light and blue light.

[0404] <Intermediate Image Screen> The imager may use an intermediate image screen. In this specification, an "intermediate image screen" is a screen on which an image is drawn. That is, in cases where the light emitted by the imager is not yet visible as an image, the imager forms a visible image on the intermediate image screen using this light. The image drawn on the intermediate image screen may be transmitted through the intermediate image screen and projected onto the laminated glass for image display of the present invention, or may be reflected by the intermediate image screen and projected onto the laminated glass for image display of the present invention.

[0405] Examples of intermediate image screens include scattering films, microlens arrays, and rear-projection screens. When a plastic material is used as the intermediate image screen, if the intermediate image screen has birefringence, the polarization plane and light intensity of polarized light incident on the intermediate image screen are disturbed, making the combiner more susceptible to color unevenness. However, using a retardation film with a predetermined phase difference can reduce this color unevenness problem. An intermediate image screen that has the function of widening and transmitting incident light is preferred, as this enables the projected image to be displayed in an enlarged scale. Examples of such intermediate image screens include screens composed of microlens arrays. Microarray lenses used in HUD systems are described, for example, in Japanese Patent Application Laid-Open No. 2012-226303, Japanese Patent Application Laid-Open No. 2010-145745, and Japanese Patent Application Laid-Open No. 2007-523369. The projector may also include a reflector that adjusts the optical path of the projected light formed by the imager.

[0406] For HUD systems using windshield glass as a projection image display member, reference can be made to Japanese Patent Application Laid-Open Nos. 2-141720, 10-096874, 2003-098470, U.S. Pat. No. 5,013,134, and Japanese Patent Publication No. 2006-512622.

[0407] The laminated glass for image displays of the present invention is particularly useful for HUD systems that use projectors with light sources such as lasers, LEDs, and OLEDs, which emit light with wavelengths that are not continuous in the visible light range. This is because the central wavelength of the selective reflection of the cholesteric liquid crystal layer can be adjusted to match each emission wavelength. It can also be used for projection of displays such as LCDs (liquid crystal displays) that emit polarized light.

[0408] <Projected Light (Incident Light)> In the image display system of the present invention, an image is projected onto the laminated glass of the present invention from a p-linearly polarized light source, thereby providing an image display system in which a viewer can view a reflected image. The direction of incidence of p-linearly polarized light is the direction in which the reflective layer included in the laminated glass of the present invention functions as a reflective polarizer for linearly polarized light. The incident light is preferably incident at an oblique incidence angle of 45 to 70° relative to the normal to the reflective layer. The Brewster angle at the interface between glass with a refractive index of approximately 1.51 and air with a refractive index of 1 is approximately 56°. By allowing p-polarized light to be incident within this angle range, the incident light for projecting an image is reflected less from the surface of the windshield glass on the viewing side toward the selective reflection layer, enabling image display with minimal double images. It is also preferable that the angle be 50 to 68°. In this case, the projected image can be observed on the side of incidence of the projection light at an angle of 45 to 70° (preferably 50 to 68°) relative to the normal to the selective reflection layer on the opposite side of the incident light.

[0409] Incident light may be incident from any direction, such as up, down, left, or right, on the laminated glass, and the angle may be determined in accordance with the viewing direction. For example, a configuration in which light is incident from below at an oblique incident angle as described above during use is preferred. Furthermore, when a retardation layer is included in the laminated glass, it is preferred that the slow axis of the retardation layer is incident at an angle of 30 to 85° or 120 to 175° relative to the vibration direction of the incident p-polarized light (the incident plane of the incident light), depending on the front retardation of the retardation layer.

[0410] As described above, the projected light when projecting an image in an image display system is preferably p-polarized light, vibrating in a direction parallel to the plane of incidence. If the light emitted from the imager is not linearly polarized, it may be made p-polarized by using a linear polarizing film disposed on the output side of the imager, or may be made p-polarized along the optical path from the imager to the laminated glass for image display. As described above, for an imager in which the polarization direction of the output light is not uniform across the wavelength ranges of red, green, and blue light, it is preferable to wavelength-selectively adjust the polarization direction so that light is incident as p-polarized light across the wavelength ranges of all colors.

[0411] The image display system may be a projection system with a variable virtual image formation position. A projection system with a variable virtual image formation position is described, for example, in Japanese Patent Application Laid-Open No. 2009-150947. By making the virtual image formation position variable, when used, for example, in a vehicle HUD system, the driver can view the virtual image more comfortably and conveniently. The virtual image formation position is a position where the virtual image can be viewed by the vehicle driver, and is typically a position 1000 mm or more away from the driver beyond the windshield glass. Here, as described in the above-mentioned Japanese Patent Application Laid-Open No. 2011-505330, if the glass is uneven (wedge-shaped) at the projected image display portion, changing the virtual image formation position requires changing the wedge angle as well. Therefore, as described, for example, in Japanese Patent Application Laid-Open No. 2017-15902, it becomes necessary to partially change the wedge angle to change the projection position and thereby simulate changes in the virtual image formation position. In a HUD system constructed using the image display system of the present invention and utilizing p-polarized light as described above, the use of wedge-shaped glass is unnecessary, and the thickness of the glass can be made uniform in the projected image display area, making it possible to suitably employ a projection system in which the virtual image formation position described above is variable.

[0412] <Irradiation Device> The irradiation device irradiates the laminated glass of the present invention with light. The output of the light irradiated from the irradiation device is desirably 1 mW or less. When the output is 1 mW or less, the irradiated light is safe even if it passes through the laminated glass and is directly observed by a person. The output of the irradiated light is preferably 0.9 mW or less, more preferably 0.8 mW or less, and even more preferably 0.7 mW or less. There is no particular lower limit for the output of the irradiated light, and it is preferable that the laminated glass is irradiated with light at a brightness of 1 cd / m 2 Preferably, the output is capable of emitting light with a brightness of 0.1 mW or more, more preferably 0.2 mW or more, and even more preferably 0.4 mW or more. The output of the irradiated light can be measured by measuring the irradiation intensity using a laser power meter (for example, "Beam Track Power Measuring Sensor 3A-QUAD" manufactured by Ophir Japan) placed 10 cm away from the light source.

[0413] The density of the irradiated light is not particularly limited, and is 0.1 mW / cm 2 More than 550 mW / cm is preferable. 2 The density of the irradiated light is preferably 0.1 mW / cm or less. 2 If the value is 550 mW / cm or more, the luminous display can be sufficiently visible at night. 2 If the density of the irradiated light is 0.2 to 530 mW / cm or less, the difference in brightness with the surroundings at night will not cause discomfort. 2 More preferably, 0.3 to 500 mW / cm 2 is more preferably 0.4 to 450 mW / cm 2 The density of the irradiated light rays can be measured by measuring the integrated amount of ultraviolet light per unit area using an ultraviolet integrating actinometer (for example, "UIT-250" manufactured by Ushio Inc.) placed at a position 10 cm away from the light source.

[0414] The diameter of the irradiated light beam is not particularly limited, but is preferably 0.005 to 3 cmφ. When the diameter of the irradiated light beam is 0.005 cmφ or more, visual recognition of light emission is possible, and when the diameter is 3 cmφ or less, a display with good contrast can be achieved. The diameter of the irradiated light beam is more preferably 0.01 to 2.5 cmφ, even more preferably 0.03 to 2 cmφ, and particularly preferably 0.05 to 1 cmφ. The diameter of the irradiated light beam can be calculated in accordance with ISO 11146 standard based on the results of measurements using a CCD sensor and a CMOS sensor (e.g., "USB 2.0 Beam Diagnostic Camera Laser Cam HR" manufactured by Coherent Japan Co., Ltd.) placed 10 cm away from the light source.

[0415] Examples of the irradiation device include a spot light source (such as "LC-8" manufactured by Hamamatsu Photonics), a xenon flash lamp (such as "CW Lamp" manufactured by Heraeus), and a black light (such as "Carry Hand" manufactured by Iuchi Seieido Co., Ltd.).

[0416] In the image display system of the present invention, when the laminated glass is irradiated with light from the irradiation device, the laminated glass has a brightness of 1 cd / m 2 It is preferable that the light emitted has a brightness of 1 cd / m or more even when irradiated with a low-intensity light beam with an output of 1 mW or less. 2 Emitting light at this luminance level enables a display with sufficient contrast, and does not dazzle a person even if the light transmitted through the laminated glass is directly observed. The luminance of the laminated glass is preferably measured at a wavelength of 400 nm or more at which the luminescence intensity of the luminescent material is greatest, or at a wavelength of 405 nm, more preferably at a wavelength of 405 nm.

[0417] The present invention will be explained in more detail below with reference to examples. The materials, reagents, amounts and proportions of substances, and procedures shown in the following examples, comparative examples, and preparation examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the following examples.

[0418] <Preparation of compositions for forming light-emitting layer> The components were mixed according to the formulations shown in Table 1 below and filtered through a polypropylene filter with a pore size of 10 μm to prepare compositions L1 and L2 for forming light-emitting layer. Note that the units of values ​​in Table 1 above are parts by mass.

[0419]

[0420] <Production of Light-Emitting Layer> The obtained composition for forming a light-emitting layer was sandwiched between polytetrafluoroethylene (PTFE) sheets, and a spacer having a thickness of 780 μm was placed between the sheets in a heat press at 150° C. and 100 kg / cm. 2 The mixture was pressed for 15 minutes under the above conditions to obtain light-emitting layers L1 and L2 having a thickness of 780 μm.

[0421] <Preparation of reflective layer-forming composition, retardation layer-forming composition, and depolarization layer-forming composition> The components were mixed according to the formulations shown in Table 2 below and filtered through a polypropylene filter with a pore size of 10 μm to prepare reflective layer-forming compositions BG1, R1, and IR1, retardation layer-forming composition A1, and depolarization layer-forming composition TW1. The blending amount of each component in the following tables is expressed in parts by mass.

[0422]

[0423] <Preparation of Composition for Forming Heat-Seal Layer> The components were mixed according to the formulation shown in Table 3 below and filtered through a polypropylene filter with a pore size of 10 μm to prepare compositions HS-1 and HS-2 for forming heat-seal layers. The blending amount of each component in the table below is expressed in parts by mass.

[0424]

[0425] <Preparation of HC layer-forming composition> The components were mixed according to the formulation shown in Table 4 below, and filtered through a polypropylene filter with a pore size of 10 μm to prepare HC layer-forming composition HC-1. The blending amount of each component in the table below is expressed in parts by mass.

[0426]

[0427] The cellulose acylate film on which the alignment film was formed was used as a transparent resin substrate.

[0428] <Saponification of Cellulose Acylate Film> A 40 μm thick cellulose acylate film was prepared by the same preparation method as in Example 20 of WO 2014 / 112575. UV-531 manufactured by Teisei Kako Co., Ltd. was added to this cellulose acylate film as an ultraviolet absorber. The amount added was 3 phr (per hundred resin). The prepared cellulose acylate film was passed through a dielectric heating roll at a temperature of 60° C. to raise the surface temperature of the film to 40° C., and then an alkaline solution having the composition shown below was applied to one side of the film using a bar coater in an amount of 14 mL / m. 2 The coating was then allowed to stand for 10 seconds under a steam-type far-infrared heater (manufactured by Noritake Co., Ltd.) heated to 110°C. Next, pure water was applied at a rate of 3 mL / m using the same bar coater. 2 Next, the film was washed with water using a fountain coater and then drained with an air knife three times, and then allowed to stay in a drying zone at 70° C. for 5 seconds to dry, thereby preparing a saponified cellulose acylate film 1.

[0429] --------------------------------------------------- Composition of alkaline solution --------------------------------------------------- Potassium hydroxide 4.7 parts by mass Water 15.7 parts by mass Isopropanol 64.8 parts by mass Surfactant (C 16 H 33 O(CHCHO) 10 H) 1.0 part by mass Propylene glycol 14.9 parts by mass

[0430] <Formation of Alignment Film> A coating solution for forming an alignment film having the composition shown below was applied to the saponified surface of the saponified cellulose acylate film 1 (transparent resin substrate) obtained above at a rate of 24 mL / m using a wire bar coater. 2 The coating was dried with hot air at 100° C. for 120 seconds to obtain an alignment film having a thickness of 0.5 μm.

[0431] -------------------------------------------------- Composition of coating liquid for forming alignment film -------------------------------------------------- 28 parts by mass of modified polyvinyl alcohol shown below 1.2 parts by mass of citric acid ester (AS3, manufactured by Sankyo Chemical Co., Ltd.) 0.84 parts by mass of photoinitiator (Irgacure 2959, manufactured by BASF) 2.8 parts by mass of glutaraldehyde 699 parts by mass of water 226 parts by mass of methanol --------------------------------------------------

[0432] (Modified polyvinyl alcohol)

[0433]

[0434] <Preparation of Reflective Layer> The alignment film prepared above was subjected to a rubbing treatment (rayon cloth, pressure: 0.1 kgf (0.98 N), rotation speed: 1000 rpm (revolutions per minute), conveying speed: 10 m / min, number of reciprocations: 1) in a direction rotated 45° clockwise with respect to the long side direction of the support.

[0435] The reflective layer-forming composition IR1 was applied to the rubbed alignment film surface at room temperature using a wire bar to a dry film thickness of 0.4 μm, yielding a coating layer. The coating layer was dried at room temperature for 30 seconds and then heated in an 85°C atmosphere for 2 minutes. The layer was then irradiated with ultraviolet light at 60% output for 6 to 12 seconds using a Fusion D-bulb (90 mW / cm lamp) at 60°C in an environment with an oxygen concentration of 1000 ppm or less, thereby fixing the cholesteric liquid crystal phase and yielding a 0.4 μm-thick cholesteric liquid crystal layer IR1. Next, the same process was repeated using a cholesteric liquid crystal layer-forming composition (BG1) to form a 0.84 μm-thick cholesteric liquid crystal layer BG1. Next, the same process was repeated using a cholesteric liquid crystal layer-forming composition (R1) to form a 0.36 μm-thick cholesteric liquid crystal layer R1 on the surface of the resulting cholesteric liquid crystal layer BG1. In this way, a film A1 having a reflective layer composed of three cholesteric liquid crystal layers was obtained. The transmission spectrum of the film A1 was measured using a spectrophotometer (V-670, manufactured by JASCO Corporation), and the transmission spectrum had selective reflection center wavelengths of 515 nm, 685 nm, and 775 nm.

[0436] <Preparation of Adhesive Layer> A heat-seal layer-forming composition HS-1 was applied to the surface of the cellulose acylate film 1 in the film A1 prepared above, opposite the reflective layer, and dried to form a heat-seal layer with a thickness of 0.8 μm. The application and curing methods were specifically as follows. The HS layer-forming composition HS-1 was applied using a wire bar so that the film would have a thickness of 0.8 μm after drying, and then dried at 120° C. for 1 minute to form a heat-seal layer, thereby preparing a film HS1 having a configuration of reflective layer / transparent resin substrate / heat-seal layer.

[0437] Composition HS-2 for forming a heat seal layer was applied to the surface of the reflective layer of the film A1 prepared above, opposite to the cellulose acylate film 1, and dried to form a heat seal layer with a thickness of 0.8 μm. Specifically, the application and curing methods were as follows. Composition HS-2 for forming a heat seal layer was applied using a wire bar so that the film thickness after drying would be 0.8 μm. Thereafter, under a nitrogen purge, an air-cooled metal halide lamp (manufactured by Eye Graphics Co., Ltd.) with an oxygen concentration of about 0.1% by volume and an illuminance of 150 mW / cm was used. 2 , irradiation amount 300mJ / cm 2 The applied curable composition for forming a heat seal layer was cured by irradiating it with ultraviolet light of 1000 W at ...

[0438] An HC layer-forming composition HC-1 was applied to the surface of the cellulose acylate film 1 of the film HS2 prepared above, opposite the reflective layer, and cured to form an HC1 layer with a thickness of 6 μm. Specifically, the application and curing methods were as follows. The HC layer-forming composition was applied at a conveying speed of 30 m / min by the die coating method using a slot die described in Example 1 of JP-A-2006-122889, and dried at an atmospheric temperature of 60°C for 60 seconds. Thereafter, under a nitrogen purge, an air-cooled metal halide lamp (manufactured by Eye Graphics Co., Ltd.) with an oxygen concentration of about 0.1% by volume and an illuminance of 150 mW / cm was used. 2 , irradiation amount 600mJ / cm 2 The applied HC layer-forming composition was cured by irradiating it with ultraviolet light of 1000 W at 100 W to form a HC layer, thereby obtaining a film HC1 having a structure of heat seal layer / reflective layer / transparent substrate layer / HC layer.

[0439] Film HC2 having a structure of reflective layer / transparent substrate layer / HC layer was obtained in the same manner as film HC1, except that film A1 was used instead of film HS1.

[0440] An adhesive layer was applied to the reflective layer side of the film HC2 prepared above. After peeling off the light release film MF-58 (adhesive layer thickness: 12 μm, manufactured by Tomoegawa Paper Co., Ltd.), the exposed adhesive layer and the reflective layer of film HC2 were attached to each other with a rubber roller under a load of 2 kg, thereby preparing film OCA1 having a configuration of protective film / adhesive layer / reflective layer / transparent resin substrate / HC layer.

[0441] <Formation of Retardation Layer> A composition A1 for forming a retardation layer was applied to the rubbed alignment film surface using a wire bar, dried, and then cured under the following conditions. A film A2 was produced in the same manner as the film A1, except that a composition IR1 for forming a reflective layer was applied on the cured retardation layer A1.

[0442] <Curing Conditions for Composition A1 for Forming Retardation Layer> After applying and drying the composition A1 for forming a retardation layer, the composition was placed on a hot plate at 50°C and heated with an electrodeless lamp "D bulb" (60 mW / cm) manufactured by Fusion UV Systems in an environment with an oxygen concentration of 1000 ppm or less. 2 ) for 6 seconds to cure the coating film. This resulted in a retardation layer whose thickness was adjusted to achieve the desired front retardation, i.e., the desired retardation. The retardation of the prepared retardation layer at 550 nm was measured using an AxoScan manufactured by Axometrics, and was found to be 126 nm.

[0443] Film HS3 having a structure of reflective layer / retardation layer / transparent resin substrate / heat seal layer was prepared in the same manner as film HS1, except that film A2 prepared above was used instead of film A1.

[0444] Film HS4 having a structure of heat seal layer / reflective layer / retardation layer / transparent resin substrate was prepared in the same manner as film HS2, except that film A2 prepared above was used instead of film A1.

[0445] Film HC3 having a structure of heat seal layer / reflective layer / retardation layer / transparent substrate layer / HC layer was obtained in the same manner as film HC1, except that film HS4 prepared above was used instead of film HS1.

[0446] Film HC4 having a structure of reflective layer / retardation layer / transparent substrate layer / HC layer was obtained in the same manner as film HC2, except that film A2 prepared above was used instead of film A1.

[0447] Film OCA2 having a structure of protective film / adhesive layer / reflective layer / retardation layer / transparent resin substrate / HC layer was produced in the same manner as film OCA1, except that film HC4 produced above was used instead of film HC2.

[0448] <Formation of Polarization Conversion Layer> Film A3 was prepared in the same manner as Film A2, except that a polarization conversion layer TW1 was applied to the cholesteric liquid crystal layer R1 to a thickness of 0.8 μm. The polarization conversion layer TW1 was prepared by applying the polarizer conversion layer-forming composition TW1 to the cholesteric liquid crystal layer R1 at room temperature using a wire bar, drying the coating at room temperature for 30 seconds, and then heating it in an 85°C atmosphere for 2 minutes. The layer was then irradiated with ultraviolet light at 60% output for 6 to 12 seconds using a Fusion D bulb (90 mW / cm lamp) at 60°C in an environment with an oxygen concentration of 1000 ppm or less, and the polarization conversion layer was fixed. The pitch number x of the helical orientation structure of the polarization conversion layer TW1 was 0.14.

[0449] Film HS5 having a structure of polarization conversion layer / reflective layer / retardation layer / transparent resin substrate / heat seal layer was prepared in the same manner as film HS1, except that film A3 prepared above was used instead of film A1.

[0450] Film HS6 having a structure of heat seal layer / polarization conversion layer / reflective layer / retardation layer / transparent resin substrate was produced in the same manner as film HS2, except that film A3 produced above was used instead of film A1.

[0451] Film HC5 having a structure of heat seal layer / polarization conversion layer / reflective layer / retardation layer / transparent substrate layer / HC layer was obtained in the same manner as film HC1, except that film A3 prepared above was used instead of film A1 and a heat seal was applied to the surface on the polarization conversion layer side instead of the reflective layer.

[0452] Film HC6 having a structure of polarization conversion layer / reflective layer / retardation layer / transparent substrate layer / HC layer was obtained in the same manner as film HC2, except that film A3 prepared above was used instead of film A1.

[0453] Film OCA3 having a structure of protective film / adhesive layer / polarization conversion layer / reflective layer / retardation layer / transparent resin substrate / HC layer was produced in the same manner as film OCA1, except that film HC6 produced above was used instead of film HC2.

[0454] <Formation of Laminated Glass> Using the light-emitting layers L1 to L2, films A1, HS1 to HS6, and OCA1 to OCA3 prepared above, laminated glasses of Examples and Comparative Examples were prepared by the following method.

[0455] Example 1: A concavely curved glass substrate measuring 260 mm long x 330 mm wide, with a curvature of 330 mm long x 1750 mm long, 260 mm short x 1250 mm wide, and 2 mm thick, was placed on the center of the glass substrate, with the heat-sealable layer surface as the contact surface. Furthermore, a light-emitting layer L1 measuring 260 mm long x 330 mm wide was placed on the reflective layer side of the film HS1, forming a laminate having a first glass substrate / heat-sealable layer / transparent resin substrate / reflective layer / light-emitting layer in this order. A concavely curved glass substrate (second glass substrate) of the same size, curvature, and thickness as above was placed on this laminate. This was maintained at 115°C and 10 kPa (0.1 atmospheres) for 1 hour, and then heated in an autoclave (manufactured by Kurihara Manufacturing Co., Ltd.) at 140°C and 1.2 MPa (12 atmospheres) for 45 minutes to remove air bubbles, thereby obtaining a laminated glass of Example 1 having a configuration of first glass substrate / heat seal layer / transparent resin substrate / reflective layer / light-emitting layer / second glass substrate.

[0456] Example 2 A 260 mm long x 330 mm wide light-emitting layer L1 was placed on a concavely curved glass substrate measuring 260 mm long x 330 mm wide, with a curvature of 330 mm in the longitudinal direction (R1750 mm), 260 mm in the transverse direction (R1250 mm), and 2 mm thick. A 220 mm long x 290 mm wide film HS-1 was placed on top of the light-emitting layer L1, with the reflective layer-side surface in contact with the light-emitting layer. A concavely curved glass substrate (second glass substrate) of the same size, curvature, and thickness as the first glass substrate was then placed on top of the film HS-1. This was then held at 115°C and 10 kPa (0.1 atm) for 1 hour, and then heated in an autoclave (manufactured by Kurihara Seisakusho) at 140°C and 1.2 MPa (12 atm) for 45 minutes to remove air bubbles, resulting in a laminated glass of Example 2 having a configuration of first glass substrate / light-emitting layer / transparent resin substrate / reflective layer / heat-seal layer / second glass substrate.

[0457] Example 3: A 260 mm x 330 mm light-emitting layer L1 was placed on a concavely curved glass substrate measuring 260 mm x 330 mm, with a curvature of 330 mm (longitudinal radius: 1750 mm), 260 mm (transverse radius: 1250 mm), and 2 mm (thickness). A second glass substrate (second glass substrate) of the same size, curvature, and thickness as the first glass substrate was placed on top of the first glass substrate. A 260 mm x 330 mm film HS2 was placed on top of the second glass substrate, with the heat-seal layer surface in contact with the film HS2, at the center of the glass substrate. This resulted in a laminate having the following order: first glass substrate / light-emitting layer / second glass substrate / heat-seal layer / reflective layer / transparent resin substrate. A 260 mm x 330 mm x 0.76 mm thick PVB film (interlayer) manufactured by Sekisui Chemical Co., Ltd. was placed on top of the laminate. Another curved glass substrate of the same size, curvature, and thickness as the first glass substrate was placed on top of the second glass substrate. This was held at 115°C and 10 kPa (0.1 atm) for 1 hour, and then heated in an autoclave (manufactured by Kurihara Manufacturing Co., Ltd.) at 140°C and 1.2 MPa (12 atm) for 45 minutes to remove air bubbles. The laminate was peeled between the PVB film and the transparent resin layer to produce a laminated glass of Example 3 having, in this order, a first glass substrate / light-emitting layer / second glass substrate / heat-seal layer / reflective layer / transparent resin substrate.

[0458] Example 4 A laminated glass of Example 4 having a first glass substrate / light-emitting layer / second glass substrate / heat-seal layer / reflective layer / transparent resin substrate / HC layer in this order was produced in the same manner as in Example 3, except that film HC1 was used instead of film HS2.

[0459] Example 5 A luminescent layer L1 measuring 260 mm in length and 330 mm in width was placed on a concavely curved glass substrate measuring 260 mm in length and 330 mm in width, with a curvature of 330 mm, a radius of 1750 mm in the longitudinal direction, 260 mm in the lateral direction, and a thickness of 2 mm. A curved glass substrate (second glass substrate) having the same size, curvature, and thickness as the above was further placed on top of the luminescent layer L1 in a concave manner. The resulting mixture was maintained at 115°C and 10 kPa (0.1 atmospheres) for 1 hour and then heated in an autoclave (manufactured by Kurihara Manufacturing Co., Ltd.) at 140°C and 1.2 MPa (12 atmospheres) for 40 minutes to remove air bubbles, thereby obtaining laminated glass A having a configuration of first glass substrate / luminescent layer / second glass substrate.

[0460] <Curved Surface Forming of Film> A 260 mm long x 330 mm wide film OCA1 was placed on a concavely curved glass substrate measuring 260 mm long x 330 mm wide, with a curvature of 330 mm long x 1750 mm R in the longitudinal direction, 260 mm short x 1250 mm R in the lateral direction, and 2 mm thick. The film OCA1, measuring 260 mm long x 330 mm wide, was placed in the center of the glass substrate with the protective film side facing the contact surface. A 260 mm long x 330 mm wide x 0.76 mm thick PVB film (interlayer) manufactured by Sekisui Chemical Co., Ltd. was then placed on top of the film OCA1. A curved glass substrate of the same size, curvature, and thickness as the film OCA1 was then placed on top of the film OCA1. This formed a laminate having, in this order, a first glass substrate / protective film / adhesive layer / reflective layer / transparent resin substrate / PVB / second glass substrate. The laminate was maintained at 140°C and 10 kPa (0.1 atmospheres) for 1 hour, and then peeled between the first glass substrate and the protective film, and between the PVB film and the HC layer, to obtain a curved film OCA1-2 having a configuration of protective film / adhesive layer / reflective layer / transparent resin substrate / HC layer.

[0461] <Preparation of Working Solution> A working solution having the composition shown below was prepared.

[0462] ------------------------------------------------------------------ Composition of application liquid -------------------------------------------------- Film application liquid (3M) 10 parts by weight Water 500 parts by weight ------------------------------------------------------------------

[0463] <Adjustment of film to curved surface> The protective film was peeled off from the adhesive layer of film OCA1-2, and the above-mentioned working liquid was sprayed onto the concave side of the laminated glass A and the surface of the adhesive layer of the curved film, and then the films were bonded so that the adhesive layer of the film faced the concave surface of the laminated glass A. The film and the laminated glass A were brought into close contact while scraping out the working liquid with a squeegee, and then dried at room temperature for 12 hours to obtain the laminated glass of Example 5, which had, in this order, first glass substrate / light-emitting layer / second glass substrate / adhesive layer / reflective layer / transparent resin substrate / HC layer.

[0464] Example 6 A laminated glass of Example 6 having a configuration of first glass substrate / light-emitting layer / transparent resin substrate / retardation layer / reflective layer / heat-seal layer / second glass substrate was obtained in the same manner as in Example 2, except that film HS3 was used instead of film HS1.

[0465] Example 7 A laminated glass of Example 7 having a configuration of first glass substrate / light-emitting layer / second glass substrate / heat seal layer / reflective layer / retardation layer / transparent resin substrate was obtained in the same manner as in Example 3, except that film HS4 was used instead of film HS2.

[0466] Example 8 A laminated glass of Example 8 having a structure of first glass substrate / light-emitting layer / second glass substrate / heat seal layer / reflective layer / retardation layer / transparent resin substrate / HC layer was obtained in the same manner as in Example 4, except that film HC3 was used instead of film HC1.

[0467] Example 9 A laminated glass of Example 9 having a structure of first glass substrate / light-emitting layer / second glass substrate / adhesive layer / reflective layer / retardation layer / transparent resin substrate / HC layer was obtained in the same manner as in Example 5, except that film OCA2 was used instead of film OCA1.

[0468] Example 10 A laminated glass of Example 10 having a configuration of first glass substrate / heat seal layer / transparent resin substrate / retardation layer / reflective layer / polarization conversion layer / light-emitting layer / second glass substrate was obtained in the same manner as in Example 1, except that Film HS5 was used instead of Film HS1.

[0469] Example 11 A laminated glass of Example 11 having a configuration of first glass substrate / light-emitting layer / transparent resin substrate / retardation layer / reflective layer / polarization conversion layer / heat-seal layer / second glass substrate was obtained in the same manner as in Example 2, except that Film HS5 was used instead of Film HS1.

[0470] Example 12 A laminated glass of Example 12 having a configuration of first glass substrate / light-emitting layer / second glass substrate / heat-seal layer / polarization conversion layer / reflective layer / retardation layer / transparent resin substrate was obtained in the same manner as in Example 3, except that Film HS6 was used instead of Film HS2.

[0471] Example 13 A laminated glass of Example 13 having a structure of first glass substrate / light-emitting layer / second glass substrate / heat-seal layer / polarization conversion layer / reflective layer / retardation layer / transparent resin substrate / HC layer was obtained in the same manner as in Example 4, except that Film HC5 was used instead of Film HC1.

[0472] Example 14 A laminated glass of Example 14 having a structure of first glass substrate / light-emitting layer / second glass substrate / adhesive layer / polarization conversion layer / reflective layer / retardation layer / transparent resin substrate / HC layer was obtained in the same manner as in Example 5, except that Film OCA3 was used instead of Film OCA1.

[0473] Example 15 A reflective layer consisting of a dielectric layer and a metal layer was formed by magnetron sputtering on a flat glass substrate measuring 260 mm long x 330 mm wide and 2 mm thick. The dielectric layer and silver layer were formed on the substrate as shown in Table 5.

[0474]

[0475] The refractive index of the Ag layer was estimated by fitting with an ellipsometer.

[0476] After the film formation was completed, the glass substrate with the reflective layer formed thereon was molded using a high-temperature automotive glass molding process so that the glass side was convex, with a curvature of 1750 mm in the longitudinal direction (330 mm) and 1250 mm in the transverse direction (260 mm). A 260 mm x 330 mm luminescent layer L1 was placed on the glass side of the molded inner glass plate, and a curved glass substrate (second glass substrate) of the same size, curvature, and thickness as above was placed on top of it in a concave manner. This was then held at 115 ° C and 10 kPa (0.1 atm) for 1 hour, and then heated in an autoclave (manufactured by Kurihara Seisakusho) at 140 ° C and 1.2 MPa (12 atm) for 45 minutes to remove air bubbles, resulting in a laminated glass of Example 15 having a configuration of first glass substrate / luminescent layer / second glass / reflective layer.

[0477] Comparative Example 1 A light-emitting layer L1 measuring 260 mm in length and 330 mm in width was placed on a concavely curved glass substrate measuring 260 mm in length, 330 mm in width, and 2 mm in thickness. A concavely curved glass substrate (second glass substrate) measuring 260 mm in length, 330 mm in width, and 2 mm in thickness was further placed on top of that. This mixture was held at 115°C and 10 kPa (0.1 atmospheres) for 1 hour and then heated in an autoclave (manufactured by Kurihara Manufacturing Co., Ltd.) at 140°C and 1.3 MPa (13 atmospheres) for 40 minutes to remove air bubbles, thereby obtaining a laminated glass of Comparative Example 1 having a configuration of first glass substrate / light-emitting layer / second glass substrate.

[0478] <Comparative Example 2> A laminated glass of Comparative Example 2 having a configuration of first glass substrate / heat seal layer / transparent resin substrate / reflective layer / light-emitting layer / second glass substrate was obtained in the same manner as in Example 1, except that L2 was used instead of L1.

[0479] The laminate prepared above was subjected to the following tests, and the test results are summarized in Table 6 below.

[0480] [Test Example 1] Evaluation of luminescence properties The laminated glasses of Examples and Comparative Examples were irradiated in a dark room with an irradiation device (power output adjustment of the light source, a dedicated bandpass filter (manufactured by Asahi Spectroscopy, "LX0405"), a rod lens (manufactured by Asahi Spectroscopy), and a fiber (manufactured by Asahi Spectroscopy) at a light output of 1 mW, a light wavelength of 405 nm, an irradiation diameter of 0.05 cmφ, and a light density of 509 mW / cm 2Using a mercury light source ("REX-250" manufactured by Asahi Spectroscopy Co., Ltd.) set so that the light was emitted to the second glass surface of the laminated glass, with the distance between the irradiation device and the center of the laminated glass being 1.0 m. The second glass surface side of the laminated glass was visually observed from a distance of 1.0 m from the laminated glass, and evaluated according to the following criteria: A: Luminescence from the laminated glass was visible. B: Luminescence from the laminated glass was not visible.

[0481] [Test Example 2] Evaluation of Projected Image Visibility The laminated glasses of the Examples and Comparative Examples were placed indoors, with an imager (iPad (registered trademark) manufactured by Apple Inc.) fixed and installed on a horizontal floor surface by adjusting the image projection angle. The laminated glass was positioned using a base so that the distance between the center of the laminated glass (image display unit) and the center of the imager was 1.0 m. The laminated glass was tilted so that the angle between the floor and the surface of the laminated glass was 30°. From a distance of 1.0 m from the laminated glass, the second glass surface of the laminated glass was visually observed so that the gray background simulating a road and the HUD display image were superimposed. The luminance LB of the gray background and the luminance LI of the white display on the imager were measured using a spectroradiometer (SR-3AR, manufactured by Topcon Technohouse Corporation), and the LI / LB ratio was 3.0. The HUD display image used displayed characters in white, green, and red, and was evaluated according to the following criteria. A to C are acceptable ranges. A: White, green, and red letters could be read clearly. B: White and green letters could be seen, and red letters could also be read. C: White and green letters could be seen, and red letters could just about be read. D: White and green letters could be seen, but the red letters were faint and unreadable. The results are shown in Table 6.

[0482] For the laminated glass of Examples 1 to 15, both light emission due to light irradiation and projected images were visible. In other words, when the laminated glass is applied to an image display system as a windshield glass, both virtual and real images can be displayed. For the laminated glass of Comparative Example 1, which does not have a reflective layer, light emission due to light irradiation was confirmed, but projected images were not visible. For the laminated glass of Comparative Example 2, which does not have a light-emitting material in the light-emitting layer, projected images were visible, but light emission due to light irradiation was not confirmed.

[0483]

[0484] DESCRIPTION OF SYMBOLS 1 outer glass 2 light-emitting layer 3 inner glass 4 reflective layer 5 adhesive layer 6 transparent resin substrate 7 hard coat (HC) layer 8 polarization conversion layer 9 retardation layer 10, 11, 12, 13, 14, 15 laminated glass

Claims

1. A laminated glass comprising: a pair of glass plates; a luminescent layer containing a luminescent material including a binder resin and at least one material selected from the group consisting of luminescent particles, luminescent pigments, and luminescent dyes; and a reflective layer.

2. The laminated glass according to claim 1, further comprising an adhesive layer.

3. The laminated glass according to claim 1, further comprising a transparent resin substrate.

4. The laminated glass according to claim 1, further comprising an adhesive layer and a transparent resin substrate, the adhesive layer, the transparent resin substrate, the reflective layer and the light-emitting layer being sandwiched between the pair of glass plates in this order.

5. The laminated glass according to claim 1, wherein the light-emitting layer is sandwiched between the pair of glass plates, and the glass plates have an adhesive layer, the reflective layer, and a transparent resin substrate in this order on the side opposite to the light-emitting layer.

6. The laminated glass according to claim 5, further comprising a hard coat layer on the side of the transparent resin substrate opposite to the reflective layer.

7. The laminated glass according to any one of claims 1 to 6, wherein the reflective layer comprises a metal layer and a dielectric layer.

8. A windshield glass comprising the laminated glass according to claim 7.

9. An image display system comprising the laminated glass according to claim 7, an imager for irradiating the laminated glass with light for projecting an image, and an irradiation device for irradiating the laminated glass with a light beam.

Citation Information

Patent Citations

  • Optical reflection film

    JP2015230477A

  • Video projection structure and video projection method

    WO2017057564A1

  • Light-emitting display, interlayer film for laminated glass, laminated glass, and light-emitting display system

    WO2018181269A1

  • Laminated structure and solar power generation system

    WO2019065922A1