Zirconia sol and method for producing zirconia sol

The zirconia sol with controlled particle size and shape, achieved by dropwise addition of ammonia water to zirconium oxychloride, addresses the limitations of existing sols by enhancing polishing efficiency and smoothness in semiconductor polishing.

WO2024203823A1PCT designated stage expired Publication Date: 2024-10-03DAIICHI KIGENSO KAGAKU KOGYO CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011247
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing zirconia sols are not suitable for precision polishing due to inadequate particle size and shape, leading to low smoothness and high surface roughness, especially in semiconductor polishing applications.

Method used

A zirconia sol with a particle diameter of 50 nm to 250 nm and a ratio of angular and distorted particles of 40% or more is produced by adding ammonia water dropwise to a zirconium oxychloride solution, controlling the concentration and volume of ammonia water, which slows down nucleus formation and promotes grain growth, resulting in larger, distorted particles.

Benefits of technology

The produced zirconia sol exhibits higher polishing rates and lower surface roughness, making it more effective as an abrasive grain for precision polishing applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011247_03102024_PF_FP_ABST
    Figure JP2024011247_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a zirconia sol that has a particle diameter D50 of 50 nm to 250 nm and a proportion X, obtained by the procedure detailed below, of at least 40%. (Procedure) A transmission electron microscope image that includes at least 20 isolated particles is obtained. The following operations (1) through (5) are performed on each of the isolated particles in the transmission electron microscope image. (1) A circumscribed circle and an inscribed circle having the same center as the circumscribed circle are obtained. (2) The ratio [(diameter of circumscribed circle) / (diameter of inscribed circle)] of the diameter of the obtained circumscribed circle and the diameter of the obtained inscribed circle is determined. (3) The ratio ([(diameter of circumscribed circle) / (diameter of inscribed circle)]) is determined for all of the isolated particles in the transmission electron microscope image. (4) The number of isolated particles A for which the ratio the ratio ([(diameter of circumscribed circle) / (diameter of inscribed circle)]) is at least 2.0 is counted. (5) The proportion X of the number of isolated particles A to the total number of isolated particles is determined.
Need to check novelty before this filing date? Find Prior Art

Description

Zirconia sol and method for producing zirconia sol

[0001] The present invention relates to a zirconia sol and a method for producing a zirconia sol.

[0002] Zirconia sol is used as a raw material powder for fine ceramics, a precision abrasive, cosmetics, a filler for paints, a zirconia thin film, etc. (see, for example, Patent Document 1).

[0003] Japanese Patent Application Publication No. 02-137732

[0004] An object of the present invention is to provide a zirconia sol that is more suitable as abrasive grains, and to provide a method for producing the zirconia sol.

[0005] The present invention provides the following: [1] Particle diameter D 50 A zirconia sol characterized in that the particle size is in the range of 50 nm to 250 nm, and the proportion X obtained by the following procedure is 40% or more. <Procedure> A transmission electron microscope image containing 20 or more isolated particles is obtained. For each isolated particle in the transmission electron microscope image, the following steps 1) to 5) are performed. 1) A circumscribing circle and an inscribing circle having the same center as the circumscribing circle are determined. 2) The ratio of the diameter of the obtained circumscribing circle to the diameter of the inscribing circle [(diameter of the circumscribing circle) / (diameter of the inscribing circle)] is determined. 3) For all isolated particles in the transmission electron microscope image, the ratio [(diameter of the circumscribing circle) / (diameter of the inscribing circle)] is determined. 4) The number of isolated particles A for which the ratio [(diameter of the circumscribing circle) / (diameter of the inscribing circle)] is 2.0 or more is counted. 5) The proportion X of the isolated particles A to all isolated particles is determined. (Proportion X (%)) = [(number of isolated particles A) / (total number of isolated particles)] x 100

[0006] Particles with the ratio [(circumscribed circle diameter) / (inscribed circle diameter)] of 2.0 or more can be said to be particles with angular, distorted shapes. According to the configuration of [1], the ratio X is 40% or more, and a certain number or more of particles with angular, distorted shapes are contained. Zirconia sol containing such particles is useful as abrasive grains. In particular, according to the configuration of [1], the particle diameter D 50In other words, according to the configuration [1], the particle diameter D 50 The particle diameter D is in the range of 50 nm to 250 nm, and a certain number of particles having angular or irregular shapes are contained therein. 50 Zirconia sols containing irregularly shaped particles with a particle size of 50 nm or more and 250 nm or less are expected to have a higher rate and higher smoothness (low surface roughness) than existing products, particularly in precision polishing of semiconductors and the like.

[0007] Furthermore, the present invention provides the following: [2] The zirconia sol according to [1] above, wherein the proportion X is 50% or more.

[0008] When the ratio X is 50% or more, the abrasive grains are more useful as polishing grains.

[0009] Furthermore, the present invention provides the following: [3] The particle diameter D 50 The zirconia sol according to [1] or [2], wherein the average particle size is 200 nm or less.

[0010] The particle diameter D 50 When the particle size is 200 nm or less, the particles are more useful as polishing abrasive grains.

[0011] Furthermore, the present invention provides the following: [4] A method for neutralizing an aqueous zirconium oxychloride solution by dropwise adding ammonia water to the aqueous zirconium oxychloride solution, wherein the concentration of the aqueous zirconium oxychloride solution is 10 mass % or more (ZrO 2 The method for producing a zirconia sol according to any one of [1] to [3], wherein the concentration of the ammonia water is 10 mass % or more, and the volume of the droplets of ammonia water dropped in the step A is 1.0 ml or less.

[0012] According to the configuration [4], ammonia water is first used as a neutralizing agent. Using ammonia water as a neutralizing agent allows the zirconia sol of the configuration [1], i.e., a zirconia sol having the ratio X of 40% or more, to be obtained. Although the reason for this is unclear, the inventors speculate that ammonia water is a weaker alkali than strong alkalis such as sodium hydroxide aqueous solution, which slows the formation of particle nuclei, resulting in larger particle sizes and more distorted shapes than when a strong alkali is used. Furthermore, according to the configuration [4], in the neutralization step A, ammonia water having a specific concentration range is dropwise added to a zirconium oxychloride aqueous solution having a specific concentration range, with the volume of the droplets controlled to a specific range. Specifically, ammonia water having a concentration of 10% by mass or more is dropwise added to a zirconium oxychloride aqueous solution having a concentration of 10% by mass or more. The volume of the ammonia water droplets added dropwise is 1.0 ml or less. This allows the zirconia sol of the configuration [1], i.e., a zirconia sol having the ratio X of 40% or more, to be obtained. Although the reason for this is unclear, the process by which zirconium oxychloride solution reacts with ammonia water to produce zirconium hydroxide is thought to be as follows: (1) The reaction of zirconium oxychloride with ammonia produces a zirconium hydroxide nucleus (chemical formula: Zr(OH) 4}n) is generated, and (2) aggregation of zirconium hydroxide nuclei and particle growth of the zirconium hydroxide nuclei proceed simultaneously. In this regard, the inventors speculate that the concentration of the initial zirconium oxychloride aqueous solution, the concentration of ammonia water, and the volume of droplets when ammonia water is added dropwise are factors that determine the nucleation rate and the density of the nuclei generated, and as a result, are factors that control the balance between aggregation of the nuclei and particle growth of the nuclei in (2). The particle properties (particle size, shape, etc.) of the zirconia sol finally obtained are thought to be determined by the particle properties (particle size, shape, etc.) of the zirconium hydroxide generated in step A. Thus, according to the configuration [4], ammonia water is used as a neutralizing agent, the concentration of the zirconium oxychloride aqueous solution is set to 10% by mass or more, the concentration of the ammonia water is set to 10% by mass or more, the ammonia water is dropwise added to the zirconium oxychloride aqueous solution, and the size of the ammonia water droplets during the dropwise addition is controlled to 1.0 ml or less. By using the zirconium hydroxide obtained as a raw material, it is possible to obtain many particles with large particle sizes and irregular shapes. That is, a zirconia sol having the ratio X of 40% or more can be obtained. On the other hand, if the concentration of the zirconium oxychloride aqueous solution is less than 10% by mass, if the concentration of the ammonia water is less than 10% by mass, or if the droplet volume during the dropwise addition of the ammonia water exceeds 1.0 ml, the balance of (2) becomes inappropriate, making it difficult to obtain the zirconia sol of [1].

[0013] According to the present invention, it is possible to provide a zirconia sol that is more suitable as abrasive grains, and also to provide a method for producing the zirconia sol.

[0014] FIG. 1 is a diagram for explaining the circumscribing circle and inscribing circle of an isolated particle in a transmission electron microscope image.

[0015] Hereinafter, embodiments of the present invention will be described. However, the present invention is not limited to these embodiments. In this specification, zirconia (zirconium oxide) is a general term and contains 10 mass % or less of impurity metal compounds including hafnia. In addition, in this specification, the expressions "contain" and "comprise" include the concepts of "contain," "comprise," "substantially consist," and "consist only of."

[0016] [Zirconia Sol] An example of the zirconia sol according to this embodiment will be described below, however, the zirconia sol of the present invention is not limited to the following example.

[0017] The zirconia sol according to this embodiment has a particle diameter D 50 is in the range of 50 nm or more and 250 nm or less, and the proportion X obtained by the following procedure is 40% or more. <Procedure> A transmission electron microscope image containing 20 or more isolated particles is obtained. For each isolated particle in the transmission electron microscope image, the following operations 1) to 5) are performed. 1) A circumscribing circle and an inscribing circle having the same center as the circumscribing circle are found. 2) The ratio of the diameter of the obtained circumscribing circle to the diameter of the inscribing circle [(diameter of the circumscribing circle) / (diameter of the inscribing circle)] is found. 3) For all isolated particles in the transmission electron microscope image, the ratio [(diameter of the circumscribing circle) / (diameter of the inscribing circle)] is found. 4) The number of isolated particles A for which the ratio [(diameter of the circumscribing circle) / (diameter of the inscribing circle)] is 2.0 or more is counted. 5) The proportion X of the isolated particles A to all isolated particles is found. (Proportion X (%)) = [(number of isolated particles A) / (total number of isolated particles)] x 100

[0018] As described above, the zirconia sol has a particle diameter D 50 The particle diameter D is in the range of 50 nm or more and 250 nm or less. 50 is preferably 200 nm or less, more preferably 180 nm or less, and even more preferably 150 nm or less. 50 is preferably 55 nm or more, more preferably 60 nm or more, and even more preferably 65 nm or more. 50is preferably 55 nm or more and 200 nm or less, more preferably 60 nm or more and 180 nm or less, and even more preferably 65 nm or more and 150 nm or less. 50 The measurement method is more specifically the method described in the Examples.

[0019] The zirconia sol has a proportion X of 40% or more, which is obtained by the following procedure. <Procedure> A transmission electron microscope image containing 20 or more isolated particles is obtained. For each isolated particle in the transmission electron microscope image, the following steps 1) to 5) are performed. 1) A circumscribing circle and an inscribing circle having the same center as the circumscribing circle are determined. 2) The ratio of the diameter of the obtained circumscribing circle to the diameter of the inscribing circle [(diameter of the circumscribing circle) / (diameter of the inscribing circle)] is determined. 3) For all isolated particles in the transmission electron microscope image, the ratio [(diameter of the circumscribing circle) / (diameter of the inscribing circle)] is determined. 4) The number of isolated particles A for which the ratio [(diameter of the circumscribing circle) / (diameter of the inscribing circle)] is 2.0 or more is counted. 5) The proportion X of the isolated particles A to all isolated particles is determined. (Proportion X (%)) = [(number of isolated particles A) / (total number of isolated particles)] x 100

[0020] The ratio X is preferably 45% or more, more preferably 50% or more, even more preferably 55% or more, and even more preferably 60% or more. The larger the ratio X, the better, for example, 99% or less, 90% or less, etc. The ratio X is preferably 45% or more and 99% or less, more preferably 50% or more and 99% or less, even more preferably 55% or more and 90% or less, and particularly preferably 60% or more and 85% or less. More specifically, the ratio X is a value obtained by the method described in the Examples.

[0021] Particles with the ratio [(circumscribed circle diameter) / (inscribed circle diameter)] of 2.0 or more can be said to be particles with angular, distorted shapes. In the zirconia sol, the ratio X is 40% or more, and a certain number or more of particles with angular, distorted shapes are contained. Zirconia sols containing such particles are useful as polishing abrasive grains. In particular, in the zirconia sol, the particle diameter D 50 In other words, the particle diameter D of the zirconia sol is in the range of 50 nm or more and 250 nm or less.50 The particle diameter D is in the range of 50 nm to 250 nm, and a certain number of particles having angular or irregular shapes are contained therein. 50 Zirconia sols containing irregularly shaped particles with a particle size of 50 nm or more and 250 nm or less are expected to have a higher rate and higher smoothness (low surface roughness) than existing products, particularly in precision polishing of semiconductors and the like.

[0022] The concentration of the zirconia sol is not particularly limited, but is usually 2 The concentration of the zirconia sol is 5% by mass or more and 80% by mass or less in terms of the total mass of the zirconia sol. When the concentration of the zirconia sol is 5% by mass or more, it is possible to prevent the zirconia concentration from decreasing when diluting with another solvent. When the concentration of the zirconia sol is 80% by mass or less, thickening of the sol is suppressed, resulting in excellent stability. The concentration of the zirconia sol is more preferably 10% by mass or more, and even more preferably 15% by mass or more. The concentration of the zirconia sol is more preferably 70% by mass or less, and even more preferably 60% by mass or less. The concentration of the zirconia sol is more preferably 10% by mass or more and 70% by mass or less, and even more preferably 15% by mass or more and 60% by mass or less.

[0023] The dispersion medium for the zirconia sol is not particularly limited, and examples thereof include water, hydrophilic organic solvents such as methanol, ethanol, 2-propanol, acetone, and ether, and mixtures of one or more of the hydrophilic organic solvents. Preferably, water (pure water or ion-exchanged water) is usually used as the dispersion medium for the zirconia sol.

[0024] The pH of the dispersion medium for the zirconia sol is not particularly limited, but is usually preferably 7 or less, and more preferably 1 to 6. When the pH of the dispersion medium for the zirconia sol is 7 or less, the pH is away from the isoelectric point of zirconia, and stability is improved.

[0025] <Polishing Performance> The zirconia sol was diluted with pure water to obtain ZrO 2When soda glass (surface roughness Ra (arithmetic mean roughness): 0.3 μm or more and 0.5 μm or less) is polished using a solution of 5.0 mass % converted as an abrasive, it is preferable that the polishing rate is 0.12 μm / min or more and the surface roughness Ra of the polished surface is 0.6 nm or less. When the polishing rate is 0.12 μm / min or more and the surface roughness Ra of the polished surface is 0.6 nm or less, a polished surface with low surface roughness can be obtained in a short time.

[0026] The polishing rate is more preferably 0.13 μm / min or more, and even more preferably 0.14 μm / min or more. As long as the surface roughness does not exceed a certain level, the higher the polishing rate, the better. Specifically, the polishing rate is more preferably 1.0 μm / min or less, and even more preferably 0.7 μm / min or less. The polishing rate is more preferably 0.12 μm / min or more and 1.0 μm / min or less, and even more preferably 0.13 μm / min or more and 0.7 μm / min or less.

[0027] The surface roughness Ra of the polished surface is more preferably 0.55 nm or less, and even more preferably 0.50 nm or less. The smaller the surface roughness Ra of the polished surface, the better, for example, 0.10 nm or more, 0.20 nm or more, etc. The surface roughness Ra of the polished surface is more preferably 0.10 nm or more and 0.55 nm or less, and even more preferably 0.20 nm or more and 0.50 nm or less.

[0028] The zirconia sol according to this embodiment can be obtained, for example, by the following method for producing a zirconia sol.

[0029] [Method for Producing Zirconia Sol] An example of a method for producing a zirconia sol will be described below, although the method for producing a zirconia sol is not limited to the following example.

[0030] The method for producing a zirconia sol according to this embodiment includes a step A of adding ammonia water dropwise to an aqueous zirconium oxychloride solution to neutralize the solution, wherein the concentration of the aqueous zirconium oxychloride solution is 10% by mass or more, the concentration of the aqueous ammonia is 10% by mass or more, and the volume of the droplets of aqueous ammonia added in the step A is 1.0 ml or less.

[0031] <Step A> First, in step A, aqueous ammonia is added dropwise to an aqueous zirconium oxychloride solution to neutralize it.

[0032] In this embodiment, ammonia water is used as a neutralizer for zirconium oxychloride. The concentration of the ammonia water is 10% by mass or more. The concentration of the ammonia water is preferably 15% by mass or more, and more preferably 20% by mass or more. There is no particular upper limit to the concentration of the ammonia water, but it may be, for example, 30% by mass or less, 28% by mass or less, etc. The concentration of the ammonia water is preferably 15% by mass or more and 30% by mass or less, and more preferably 20% by mass or more and 28% by mass or less.

[0033] The concentration of the zirconium oxychloride aqueous solution is 10% by mass or more. The concentration of the zirconium oxychloride aqueous solution is preferably 15% by mass or more, and more preferably 18% by mass or more. There is no particular upper limit to the concentration of the zirconium oxychloride aqueous solution, but it is, for example, 28% by mass or less, 25% by mass or less, etc. The concentration of the zirconium oxychloride aqueous solution is preferably 15% by mass or more and 28% by mass or less, and more preferably 18% by mass or more and 25% by mass or less.

[0034] The volume of the droplet of ammonia water dropped in step A is 1.0 ml or less. The volume of the droplet is preferably 0.7 ml or less, more preferably 0.5 ml or less. The smaller the volume of the droplet, the more preferable it is, for example, 0.05 ml or more, 0.1 ml or more, etc. The volume of the droplet is preferably 0.05 ml or more and 0.7 ml or less, more preferably 0.1 ml or more and 0.5 ml or less.

[0035] The dropwise addition time of the aqueous ammonia in step A is not particularly limited, but is preferably 10 minutes or more and 120 minutes or less, for example, when 1000 ml of aqueous ammonia is dropwise added to 1000 ml of an aqueous zirconium oxychloride solution. The dropwise addition time is more preferably 90 minutes or less, and even more preferably 60 minutes or less. The dropwise addition time is not particularly limited as long as it is within a range in which the reaction proceeds moderately, and is, for example, 15 minutes or more, 20 minutes or more, etc. The dropwise addition time is preferably 15 minutes or more and 90 minutes or less, and more preferably 20 minutes or more and 60 minutes or less.

[0036] The temperatures of the aqueous zirconium oxychloride solution and the aqueous ammonia before performing step A are not particularly limited, and may be, for example, ambient temperature (for example, in the range of 20°C to 40°C). The temperatures of the aqueous zirconium oxychloride solution and the aqueous ammonia before performing step A may be adjusted in advance. When adjusting the temperatures, the temperatures of the aqueous zirconium oxychloride solution and the aqueous ammonia before performing step A are preferably 50°C or lower, more preferably 40°C or lower. When adjusting the temperatures, the lower limits of the temperatures of the aqueous zirconium oxychloride solution and the aqueous ammonia before performing step A are not particularly limited as long as they are within a range in which the reaction proceeds appropriately, and are, for example, 5°C or higher, 10°C or higher, etc. When adjusting the temperatures, the temperatures of the aqueous zirconium oxychloride solution and the aqueous ammonia before performing step A are preferably 5°C to 50°C, more preferably 10°C to 40°C.

[0037] According to the above-described method for producing a zirconia sol, ammonia water is used as a neutralizing agent, thereby enabling the production of the zirconia sol, i.e., a zirconia sol having the ratio X of 40% or more. Furthermore, according to the above-described method for producing a zirconia sol, in the neutralization step A, ammonia water having a concentration of 10% by mass or more is added dropwise to a zirconium oxychloride aqueous solution having a concentration of 10% by mass or more, and the volume of the ammonia water droplets added dropwise is 1.0 ml or less, thereby obtaining many particles with large particle sizes and irregular shapes. That is, a zirconia sol having the ratio X of 40% or more can be obtained. According to the above-described method for producing a zirconia sol, ammonia water is used as a neutralizing agent, the concentration of the zirconium oxychloride aqueous solution is 10% by mass or more, the concentration of the ammonia water is 10% by mass or more, and the volume of the ammonia water droplets added dropwise is 1.0 ml or less, thereby obtaining many particles with large particle sizes and irregular shapes. That is, a zirconia sol having the ratio X of 40% or more can be obtained.

[0038] After step A, the mixture is stirred and homogenized as necessary, thereby obtaining a precipitate of zirconium hydroxide. The stirring time is not particularly limited, and is, for example, from 15 minutes to 120 minutes.

[0039] Thereafter, the zirconium hydroxide is washed as necessary. The washing is performed, for example, until the Cl concentration becomes a predetermined concentration or less. The predetermined concentration is preferably, for example, 0.01% or less. The washing method is not particularly limited, but an example thereof is a method in which the zirconium hydroxide is filtered and dispersed in ion-exchanged water repeatedly.

[0040] Next, an acid is added as a deflocculating agent. The deflocculating agent for zirconium hydroxide is not particularly limited as long as it is a water-soluble inorganic or organic acid, and examples thereof include hydrochloric acid, nitric acid, sulfuric acid, acetic acid, lactic acid, citric acid, tartaric acid, malic acid, and mandelic acid. However, even if hydrochloric acid or nitric acid is present in excess in the zirconia sol, it can be easily removed by purifying with water after the zirconia sol is produced, and therefore, the amount of the deflocculating agent to be added is preferably in the range of 1: acid / ZrO 2(molar ratio) = 0.01 or more and 3 or less, more preferably 0.1 or more and 1.5 or less. 2 When the molar ratio of the acid to ZrO is 0.01 or more, the zirconium hydroxide can be sufficiently peptized. 2 Even if the molar ratio exceeds 3, the quantitative effect is small. 2 When the molar ratio is 3 or less, it is economical.

[0041] Next, heating and aging are performed to peptize the zirconium hydroxide. From the viewpoint of yield, the heating and aging temperature is preferably 80°C or higher, more preferably 90°C or higher. The heating temperature is preferably 110°C or lower, more preferably 105°C or lower. The heating temperature is preferably 80°C or higher and 110°C or lower, more preferably 90°C or higher and 105°C or lower. From the viewpoint of yield, the heating and aging time is preferably 24 hours or higher, more preferably 48 hours or higher. The heating and aging time is preferably 120 hours or lower, more preferably 100 hours or lower. The heating and aging time is preferably 24 hours or higher and 120 hours or lower, more preferably 48 hours or higher and 100 hours or lower.

[0042] After that, the zirconia sol may be concentrated by ultrafiltration after cooling to room temperature. Excess acid can be easily removed by ultrafiltration.

[0043] The method for producing zirconia sol according to this embodiment has been described above.

[0044] The present invention will be described in detail below using examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention. Note that the zirconia sol in the examples and comparative examples contains 1 to 3 mass % of hafnium as an inevitable impurity relative to zirconium (calculated using the following formula (X)). <Formula (X)> ([mass of hafnium oxide] / ([mass of zirconium oxide]+[mass of hafnium oxide]))×100(%)

[0045] The maximum and minimum values ​​of the content of each component shown in the following examples should be considered as the preferred minimum and maximum values ​​of the present invention, regardless of the content of other components. Also, the maximum and minimum values ​​of the measured values ​​shown in the following examples should be considered as the preferred minimum and maximum values ​​of the present invention, regardless of the content (composition) of each component.

[0046] [Preparation of Zirconia Sol] (Example 1) An aqueous solution of zirconium oxychloride (ZrO 2 To 1,000 g of ammonia water (10% by mass, calculated as 10% by mass), 1,380 g of ammonia water (10% by mass), also adjusted to 25°C, was added dropwise over 30 minutes. The number of liquid delivery tubes and the rate of addition were adjusted so that the volume of the ammonia water droplets was in the range of 0.1 to 0.5 ml. Stirring was then continued for 30 minutes to obtain a precipitate of zirconium hydroxide. The zirconium hydroxide was separated by filtration and dispersed again in ion-exchanged water, a washing procedure that was repeated. This procedure was repeated until the Cl concentration reached 0.01% or less. The concentration of zirconium hydroxide after washing was ZrO 2 300 g of the obtained zirconium hydroxide was mixed with 299 g of ion-exchanged water and 39.1 g of nitric acid (60 mass %) to prepare a slurry, which was maintained at 100°C under reflux for 48 hours while stirring, and the obtained zirconia sol precursor was purified using ultrafiltration, thereby obtaining the zirconia sol according to Example 1.

[0047] (Examples 2 to 4, Comparative Example 1) Zirconia sols according to Examples 2 to 4 and Comparative Example 1 were obtained in the same manner as Example 1, except that the concentration of the zirconium oxychloride aqueous solution and / or the concentration of aqueous ammonia was changed as shown in Table 1. In Table 1, "ZOC" means zirconium oxychloride. (Comparative Examples 2 to 3) Zirconia sols according to Comparative Examples 2 to 3 were obtained in the same manner as Example 1, except that the concentration of the zirconium oxychloride aqueous solution and / or the concentration of aqueous ammonia, and the volume of the aqueous ammonia droplets were changed as shown in Table 1.

[0048] Comparative Example 4 A zirconia sol according to Comparative Example 4 was obtained in the same manner as in Example 2, except that 15 mass % caustic soda (aqueous sodium hydroxide solution) was used instead of the ammonia water.

[0049] (Comparative Example 5) ZrO 2 A zirconia sol according to Comparative Example 5 was obtained in the same manner as in Example 1, except that a zirconia sol precursor was used, which was obtained by holding an aqueous solution of zirconium oxychloride diluted with pure water to a concentration of 1% by mass in terms of sol content under reflux at 100°C for 60 hours.

[0050] [Particle diameter D 50 Measurement of ZrO 2 The resulting solution was diluted to 0.1% by mass in terms of the total mass of the zirconia sol, and then placed in a dynamic light scattering particle size distribution measuring device ("Zetasizer Nano ZS" manufactured by Malvern Panalytical) to measure the particle diameter D of the zirconia sol. 50 The results are shown in Table 1. <Measurement conditions> Measurement temperature: 25°C Scattering angle: 173° Dispersoid: ZrO 2 Dispersion medium: Water Cell: Genuine disposable cell

[0051] [Measurement of Particle Shape] First, TEM images (transmission electron microscope images) of the zirconia sols of the Examples and Comparative Examples were obtained. A transmission electron microscope (Hitachi, Ltd., product name: HV-8100) was used to capture the TEM images, with a field of view of 1.15 μm × 0.90 μm. Next, the number of isolated particles was counted visually. Specifically, the number of particles whose circumscribed circles had a diameter of 50 nm or more was counted. When multiple circumscribed circles existed around a particle, the one with the smallest ratio (see "2" below) between the diameter of the circumscribed circle and the diameter of the inscribed circle (concentric inscribed circle) with the same center as the circumscribed circle was adopted. Note that particles whose circumscribed circles had a diameter of less than 50 nm were not counted because such particles have low effectiveness as abrasives. When the number of isolated particles was 20 or more, the TEM image was used as the image to be evaluated. If the number of isolated particles was less than 20, a TEM image of a different field of view was taken, and this process was repeated until a TEM image containing 20 or more isolated particles was obtained. The following operations were performed on each isolated particle (the isolated particles to be counted) in the obtained TEM image. 1) First, the circumscribing circle of the particle and the inscribing circle (concentric inscribing circle) with the same center as the circumscribing circle were determined (see Figure 1). The definitions of the circumscribing circle and the inscribing circle are the same as those in the MCC method of circularity in JIS B 7451:1997. 2) Next, the ratio of the diameter of the obtained circumscribing circle to the diameter of the inscribing circle [(diameter of the circumscribing circle) / (diameter of the inscribing circle)] was calculated. 3) The ratio [(diameter of the circumscribing circle) / (diameter of the inscribing circle)] was calculated for all isolated particles in the TEM image (all isolated particles to be counted). 4) The number of isolated particles (hereinafter also referred to as "isolated particles A") with a ratio [(circumscribed circle diameter) / (inscribed circle diameter)] of 2.0 or more was counted. 5) The proportion of isolated particles A to all isolated particles (all isolated particles counted) (hereinafter also referred to as "proportion X") was calculated. (Proportion X (%)) = [(number of isolated particles A) / (total number of isolated particles)] x 100. The results are shown in Table 1.

[0052] [Polishing Performance Evaluation] The zirconia sols of the Examples and Comparative Examples were diluted with pure water to obtain ZrO 2A solution of 5.0% by mass (calculated as a polishing agent) was used to polish soda glass (Ra: 0.3 to 0.5 μm), and the polishing rate and the surface roughness Ra of the polished surface were measured. The polishing conditions were as follows: Substrate (object to be polished): soda glass (surface roughness Ra (arithmetic mean roughness): 0.3 μm or more and 0.5 μm or less) Polishing apparatus: single-sided polishing apparatus (EJ-380N manufactured by ENGIS) Polishing pad: suede-type pad Polishing load: 100 g / cm2 (9.8 kPa) Rotation speed of platen: 80 rpm (linear speed: 9.5 m / min) Polishing time: 15 minutes Supply rate of polishing composition: 10 mL / min Measured area of ​​object to be polished: 0.143 × 0.107 mm (surface roughness) Pitch: 0.164 μm

[0053] The polishing rate was measured by measuring the weight of the substrate before and after polishing and calculating the difference. The surface roughness (arithmetic mean roughness (Ra)) of the polished surface of the object to be polished after polishing was measured using a non-contact 3D shape measurement / surface roughness measurement instrument "NewView5032" manufactured by AMETEC Corporation under the condition of a viewing angle of 0.143 × 0.107 mm. The results are shown in Table 1.

[0054]

Claims

1. Particle size D 50 A zirconia sol characterized in that the diameter of the zirconia sol is within a range of 50 nm or more and 250 nm or less, and the proportion X obtained by the following procedure is 40% or more. <Procedure> A transmission electron microscope image containing 20 or more isolated particles is obtained. For each isolated particle in the transmission electron microscope image, the following operations 1) to 5) are performed. 1) A circumscribing circle and an inscribing circle having the same center as the circumscribing circle are obtained. 2) A ratio of the diameter of the obtained circumscribing circle to the diameter of the inscribing circle [(diameter of the circumscribing circle) / (diameter of the inscribing circle)] is obtained. 3) For all isolated particles in the transmission electron microscope image, the ratio [(diameter of the circumscribing circle) / (diameter of the inscribing circle)] is obtained. 4) The number of isolated particles A having a ratio [(diameter of the circumscribing circle) / (diameter of the inscribing circle)] of 2.0 or more is counted. 5) A proportion X of the isolated particles A to all isolated particles is obtained. (Proportion X (%))=[(number of isolated particles A) / (total number of isolated particles)]×100 2. The zirconia sol according to claim 1, wherein the ratio X is 50% or more.

3. The particle diameter D 50 3. The zirconia sol according to claim 1, wherein the average particle diameter is 200 nm or less.

4. A method for producing a zirconia sol as described in claim 1 or 2, characterized in that it comprises a step A of adding ammonia water dropwise to an aqueous zirconium oxychloride solution to neutralize it, wherein the concentration of the aqueous zirconium oxychloride solution is 10 mass% or more, the concentration of the ammonia water is 10 mass% or more, and the volume of the droplets of ammonia water dropped in step A is 1.0 ml or less.

Citation Information

Patent Citations

  • Production of aqueous weakly acidic crystallized zirconia-based sol

    JP1990137732A

  • Calcium zirconate-based powder and method for producing the same

    JP2021075413A

  • Zirconia sol and method for producing the same

    JP5019826B2