Ɑ-type sialon fluorescent body and light-emitting device

The α-type sialon phosphor with a specific composition and hydrogen annealing process addresses the challenges of luminescent property optimization and thermal expansion, enhancing its efficiency in converting blue light to longer wavelengths for improved white LED performance.

WO2024203901A1PCT designated stage expired Publication Date: 2024-10-03DENKA CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011396
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current α-type sialon phosphors face challenges in achieving optimal luminescent properties and thermal expansion coefficients for efficient wavelength conversion in white LEDs, particularly in maintaining fluorescence efficiency across a wide wavelength range from ultraviolet to blue light.

Method used

Development of an α-type sialon phosphor with a specific general formula (Ca_x, Eu_y)(Si_12-(m+n)Al_m+n)(O_nN_16-n) that has a controlled average linear expansion coefficient between 4.2 ppm/°C and 4.6 ppm/°C, optimized lattice constants, and a hydrogen annealing process to enhance luminescent characteristics.

Benefits of technology

The optimized α-type sialon phosphor exhibits improved luminescent properties, including efficient fluorescence emission and controlled thermal expansion, facilitating better performance in white LEDs by converting blue light into longer wavelengths effectively.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011396_03102024_PF_FP_ABST
    Figure JP2024011396_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This α-type sialon fluorescent body is represented by the general formula (Cax, Euy)(Si12-(m+n)Alm+n)(OnN16-n), and has an average coefficient of linear expansion α' at 25-900 °C of 4.2 ppm / °C to 4.6 ppm / °C. In the general formula, 0<x<2.0, 0<y≤0.5, 0.3≤x+y≤2.0, 0<m≤4.0, and 0<n≤3.0 are satisfied.
Need to check novelty before this filing date? Find Prior Art

Description

α-type sialon phosphor and light-emitting device

[0001] The present invention relates to an α-sialon phosphor and a light-emitting device.

[0002] An α-sialon phosphor activated with a rare earth element such as Eu can efficiently convert blue light into long wavelength light, and is therefore used as a wavelength conversion material for white LEDs, for example.

[0003] α-SiAlON phosphors usually have a structure in which the Si-N bonds of α-SiN crystals are partially replaced with Al-N bonds and Al-O bonds, and in order to maintain electrical neutrality, specific elements (Ca, Li, Mg, Y, or lanthanide metals excluding La and Ce) intercalate and form a solid solution between the crystal lattice. Fluorescent properties are exhibited by using rare earth elements as the luminescence center as some of the intercalated and solid-solved elements. In particular, α-SiAlON phosphors in which Ca is solid-solved and part of it is substituted with Eu are excited relatively efficiently in a wide wavelength range from ultraviolet to blue, and emit yellow or orange light.

[0004] In order to further improve the fluorescent properties of α-sialon phosphors, various attempts have been proposed (for example, Patent Documents 1 to 3).

[0005] Japanese Patent Publication No. 2009-96882 Japanese Patent No. 6667025 Japanese Patent No. 6785333

[0006] With the widespread use of white LEDs, the performance required of α-sialon phosphors is becoming increasingly higher.

[0007] The present inventors have now conducted various investigations in order to obtain an α-sialon phosphor having improved luminescence properties.

[0008] The present inventors have completed the invention provided below through various investigations.

[0009] 1. An α-sialon phosphor represented by the following general formula, having an average linear expansion coefficient α' of 4.2 ppm / °C or more and 4.6 ppm / °C or less at 25 to 900°C. General formula: (Ca x , Eu y ) (Si 12-(m+n) Al m+n ) (O n N16-n In the general formula, x, y, m, and n satisfy the following: 0<x<2.0 0<y≦0.5 0.3≦x+y≦2.0 0<m≦4.0 0<n≦3.0 2. The α-sialon phosphor according to 1., wherein 2.5≦m≦4.0 and 0<n≦0.5. 3. The α-sialon phosphor according to 1. or 2., wherein the average linear expansion coefficient at 25 to 300°C is α 1 ', and the average linear expansion coefficient at 700 to 900°C is α 2 ´, then α 2 ´ / α 1 4. An α-sialon phosphor according to any one of 1. to 3., wherein the lattice constant a of the unit lattice is 1.3 to 1.8 at 25°C. 25 is 7.900 Å or more and 7.960 Å or less, and the lattice constant c 25 5. An α-sialon phosphor according to any one of 1. to 4., wherein the lattice volume V of a unit cell at 25°C is 25 is 308 Å 3 More than 320 Å 3 6. An α-sialon phosphor as set forth in any one of 1. to 5., wherein in the general formula, x, y, m, and n satisfy the following: 1.3≦x<2.0 0.01≦y≦0.1 1.3≦x+y≦2.0 2.8≦m<4.0 0.1≦n≦0.27 7. A light emitting device comprising: a light emitting element; and a wavelength conversion unit containing the α-sialon phosphor as set forth in any one of 1. to 6., which converts the wavelength of light emitted from the light emitting element to a longer wavelength.

[0010] According to the present invention, an α-sialon phosphor having improved luminescence properties is provided.

[0011] 1 is a schematic cross-sectional view illustrating the structure of a light-emitting device.

[0012] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. The drawings are for illustrative purposes only. The shapes and dimensional ratios of the components in the drawings do not necessarily correspond to the actual products.

[0013] In this specification, unless otherwise specified, the expression "X to Y" in the description of a numerical range means at least X and at most Y. For example, "1 to 5% by mass" means "at least 1% by mass and at most 5% by mass."

[0014] <α-type Sialon phosphor> The α-type Sialon phosphor of the present embodiment is a phosphor represented by the general formula: (Ca x , Eu y ) (Si 12-(m+n) Al m+n ) (O n N 16-n In the above general formula, x, y, m, and n satisfy the following: 0<x<2.0 0<y≦0.5 0.3≦x+y≦2.0 0<m≦4.0 0<n≦3.0

[0015] Moreover, the average linear expansion coefficient α' of the α-sialon phosphor of this embodiment at 25 to 900°C is 4.2 ppm / °C or more and 4.6 ppm / °C or less.

[0016] The α-sialon phosphor of this embodiment has good light-emitting properties. Although the reason for this is not entirely clear, it is presumed that the α-sialon phosphor of this embodiment has a crystal structure that easily emits fluorescence efficiently, taking into consideration that m and n in the above general formula are within specific numerical ranges and that the thermal expansion coefficient is considered to be an index that can correlate with the crystal structure.

[0017] In this embodiment, the average linear expansion coefficient α' can be determined by measuring and analyzing the relationship between temperature and lattice constant, for example, as shown in the following [Example of procedure for determining the average linear expansion coefficient α']. For details on how to determine the average linear expansion coefficient α', please refer to the examples below.

[0018] [Example of procedure for determining the average linear expansion coefficient α'] (1) X-ray diffraction measurement of an α-sialon phosphor is performed at several points within the temperature range of 25 to 900°C. (2) From the results of the X-ray diffraction measurement, the lattice constant of the crystal in the phosphor at each temperature T is determined. In the case of an α-sialon phosphor, the lattice constant a T and c T In the crystal structure of α-sialon, the lattice constant b T is a T (3) Temperature T - lattice constant a T , temperature T - lattice constant c T (4) From the approximate lines, the lattice constant a at 25°C is calculated. 25 and c 25 , and the lattice constant a at 900 ° C. 900 and c 900 These values ​​are used as V in formula 1 below. 25 and V 900 Substituting into the formula, the lattice volume V at 25 ° C. 25 and the lattice volume V at 900 ° C. 900 Then, the volume expansion coefficient β is calculated based on the following formula 2.

[0019]

[0020]

[0021] (5) Calculate the average linear expansion coefficient α' using the formula α' = β / 3. This formula α' = β / 3 is used to calculate the average linear expansion coefficient of a polycrystalline body, assuming that the sample is an isotropic material.

[0022] The α-sialon phosphor of this embodiment can be produced by using appropriate raw materials in appropriate amounts and by adopting appropriate manufacturing conditions. "Using appropriate materials in appropriate amounts" refers to adjusting the amounts of raw materials so that x, y, m, and n in the general formula above are satisfied. "Appropriate manufacturing conditions" refer to an "annealing step" in an inert gas atmosphere such as nitrogen gas, and a "hydrogen annealing step" in a hydrogen gas atmosphere, which will be described in detail later. The α-sialon phosphor of this embodiment can be produced by adopting appropriate manufacturing methods and manufacturing conditions. Conversely, if appropriate manufacturing methods and manufacturing conditions are not adopted, the α-sialon phosphor of this embodiment may not be obtained even if appropriate raw materials are used in appropriate amounts.

[0023] The α-sialon phosphor of this embodiment will be described further.

[0024] (General formula: (Ca x , Eu y ) (Si 12-(m+n) Al m+n ) (O n N 16-n )) x is sufficient to satisfy 0<x<2.0, preferably 1.0≦x<2.0, and more preferably 1.3≦x<2.0; y is sufficient to satisfy 0<y<0.5, and preferably 0.01≦y≦0.1; x+y is sufficient to satisfy 0.3≦x+y≦2.0, and preferably 1.0≦x+y≦2.0, and more preferably 1.3≦x+y≦2.0; m is sufficient to satisfy 0<m≦4.0, and preferably 2.5≦m≦4.0, more preferably 2.8≦m≦4.0, and even more preferably 2.8≦m<4.0; n is sufficient to satisfy 0<n≦3.0, and preferably 0<n≦0.5, more preferably 0.1≦n≦0.4, and even more preferably 0.1≦n≦0.27.

[0025] Particularly preferred numerical ranges for x, y, x+y, m, and n are as follows: 1.3≦x<2.0, 0.01≦y≦0.1, 1.3≦x+y≦2.0, 2.8≦m<4.0, 0.1≦n≦0.27.

[0026] Optimizing x, y, x+y, m, and n may further improve the luminescence characteristics of the α-sialon phosphor, and may also facilitate more appropriate control of the average linear expansion coefficient α'.

[0027] (Regarding Lattice Constant and Lattice Volume) The lattice constant a of the unit lattice of the α-sialon phosphor of this embodiment at 25° C. 25 is preferably 7.900 Å or more and 7.960 Å or less, and the lattice constant c 25 is preferably 5.720 Å or more and 5.780 Å or less. In the crystal structure of α-sialon, the lattice constant b 25 is a 25 In addition, the lattice volume V of the unit cell of the α-sialon phosphor of this embodiment at 25° C. 25 is preferably 308 Å 3 More than 320 Å 3 As described above, the α-sialon of this embodiment is presumed to have a crystal structure that is likely to efficiently emit fluorescence. The numerical ranges of these lattice constants are considered to reflect the "crystal structure that is likely to efficiently emit fluorescence." Each of the above values ​​can be determined by the Pawley method.

[0028] (Regarding the average linear expansion coefficient at low temperatures and the average linear expansion coefficient at high temperatures) In the α-sialon phosphor of this embodiment, if the average linear expansion coefficient at low temperatures and the average linear expansion coefficient at high temperatures are within appropriate numerical ranges, the light-emitting characteristics may be further improved. Specifically, if the average linear expansion coefficient at 25 to 300°C of the α-sialon phosphor of this embodiment is within the range of α 1 ', and the average linear expansion coefficient at 700 to 900°C is α 2 ´, then α 2 ´ / α 1 ' is preferably 1.3 to 1.8, more preferably 1.3 to 1.7, and even more preferably 1.3 to 1.6.

[0029] Below, α 1 ´ and α 2 The method for calculating ´ will be explained in detail below.

[0030] ・Average linear expansion coefficient α between 25 and 300°C 1 (1) Lattice constant a obtained by the Pawley method 25 , c 25 (The definitions of these symbols are the same as above) are substituted into the following equation to obtain the lattice volume V at 25 ° C. 25 Incidentally, since the crystal structure of α-sialon is hexagonal, the lattice volume is expressed by this formula.

[0031]

[0032] (2) Similarly, the lattice constant a at 300°C 300 , c 300 Using the value of , the lattice volume V at 300 ° C. 300 Calculate.

[0033] (3) The volume expansion coefficient β 1 ΔT is calculated as 300°C - 25°C = 275°C.

[0034]

[0035] (4) Assuming that the sample is an isotropic material, the average linear expansion coefficient α of the polycrystalline material is 1 ´, α 1 ´=β 1 Calculate using the formula: / 3.

[0036] ・Average linear expansion coefficient α at 700 to 900°C 2 (1) Using the Pawley method, the lattice constant a at 700°C 700 , c 700 The value is substituted into the following formula to obtain the lattice volume V at 700°C. 700 Incidentally, since the crystal structure of α-sialon is hexagonal, the lattice volume is expressed by this formula.

[0037]

[0038] (2) Similarly, the lattice constant a at 900°C 900 , c 900 Then, calculate the lattice volume V at 900 °C. 900 Calculate.

[0039] (3) Using the following formula, the volume expansion coefficient β2 ΔT is calculated as 900°C - 700°C = 200°C.

[0040]

[0041] (4) Assuming that the sample is an isotropic material, the average linear expansion coefficient α of the polycrystalline material is 2 ´, α 2 ´=β 2 Calculate using the formula: / 3.

[0042] (Regarding Properties) The α-sialon phosphor of this embodiment is typically in powder form. The lower limit of the median diameter D50 of the powdered α-sialon phosphor particles is preferably 1 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more. The upper limit of the median diameter D50 is preferably 30 μm or less, more preferably 20 μm or less. That is, the median diameter D50 is preferably 1 to 30 μm, more preferably 5 to 30 μm, and even more preferably 10 to 20 μm. By setting the median diameter D50 to 5 μm or more, the transparency of the composite described below can be further improved. On the other hand, by setting the median diameter D50 to 30 μm or less, chipping can be suppressed when cutting the composite with a dicer or the like. The median diameter D50 can be determined by a laser diffraction scattering method in accordance with JIS R1629:1997. For more specific measurement methods, see the examples below.

[0043] <Method for manufacturing α-sialon phosphor> As described above, the α-sialon phosphor of this embodiment can be manufactured by using appropriate raw materials in appropriate amounts and by adopting appropriate manufacturing conditions. An example of the manufacturing method will be described below.

[0044] Mixing of Raw Materials: First, raw materials containing the elements that constitute the Eu-containing α-sialon phosphor particles are mixed. In α-sialon phosphor particles with a low oxygen content synthesized using calcium nitride as the calcium raw material, calcium is dissolved at a high concentration. When the Ca solid solution concentration is particularly high, a phosphor is obtained that has an emission peak wavelength on the longer wavelength side (590 nm or more, more specifically, 590 nm to 610 nm, and even more specifically, 592 nm to 608 nm) compared to conventional compositions using oxide raw materials.

[0045] Other examples of raw material powders include silicon nitride, aluminum nitride, and Eu compounds. Eu compounds include europium oxide, compounds that become europium oxide after heating, and europium nitride. Europium nitride is preferred because it can reduce the amount of oxygen in the system.

[0046] An appropriate amount of pre-synthesized α-sialon phosphor particles may be added to the raw material powder. These phosphor particles may act as starting points for grain growth, and may result in α-sialon phosphor particles with a relatively large minor axis diameter. Furthermore, by changing the shape of the α-sialon particles to be added, it may be possible to control the grain shape.

[0047] Methods for mixing the raw materials include dry mixing and wet mixing in an inert solvent that does not substantially react with the raw material components, followed by removal of the solvent. Mixing devices include V-type mixers, rocking mixers, ball mills, and vibration mills. Mixing calcium nitride, which is unstable in air, is preferably carried out in a glove box with an inert atmosphere, since its hydrolysis and oxidation affect the properties of the synthesized product.

[0048] Heat Treatment (Firing) The powder obtained by mixing (hereinafter simply referred to as raw material powder) is filled into a container made of a material that is low in reactivity with the raw materials and the phosphor to be synthesized, such as a boron nitride container. Then, the mixture is heated for a predetermined time in a nitrogen atmosphere. In this way, an α-sialon phosphor can be obtained. The heat treatment temperature is preferably 1650°C or higher and 1950°C or lower. By setting the heat treatment temperature to 1650°C or higher, the amount of remaining unreacted products can be suppressed, and primary particles can be grown sufficiently. Furthermore, by setting the heat treatment temperature to 1950°C or lower, significant sintering between particles can be suppressed.

[0049] It is preferable that the raw material powder be packed into the container in a bulky manner from the viewpoint of suppressing interparticle sintering during heating. Specifically, when packing the raw material powder into the container, the bulk density is set to 0.6 g / cm 3 It is preferable to do the following:

[0050] The heating time in the heat treatment is preferably in the range of 2 hours to 24 hours, which is a time range that does not cause inconveniences such as the presence of a large amount of unreacted matter, insufficient growth of primary particles, or sintering between particles.

[0051] The above-described process produces an α-sialon phosphor having an ingot-shaped outer shape. This ingot-shaped α-sialon phosphor is then subjected to a pulverization process using a pulverizer such as a crusher, mortar grinder, ball mill, vibration mill, or jet mill, followed by a sieve classification process, to obtain a powdered α-sialon phosphor with an adjusted secondary particle size. Furthermore, the particle size of the secondary particles can be adjusted by dispersing the phosphor in an aqueous solution and removing secondary particles that are small in particle size and do not easily settle.

[0052] Annealing Step In this embodiment, the powdered α-sialon phosphor obtained through the heat treatment is preferably heated (annealed) in a nitrogen atmosphere. In this specification, this heat treatment in a nitrogen atmosphere is referred to as the "annealing step." The heating temperature in the annealing step is preferably 1300 to 1600°C, more preferably 1400 to 1500°C. Heating temperatures of 1600°C or higher are undesirable because they may cause decomposition of the α-sialon and volatilization of the luminescence center Eu. Heating temperatures of 1300°C or lower are also undesirable because they may not sufficiently improve crystallinity. The heating temperature in the annealing step is preferably lower than the heating temperature in the heating step (firing) described above.

[0053] The pressure in the annealing step is preferably atmospheric pressure or near atmospheric pressure, specifically 0.02 to 0.9 MPa (gauge pressure). The time for the annealing step is preferably 5 to 20 hours, more preferably 10 to 18 hours.

[0054] Hydrogen Gas Annealing Step After the annealing step, the processed product obtained in the annealing step is heat-treated in a hydrogen gas atmosphere. In this specification, this step is referred to as the "hydrogen gas annealing step." In the hydrogen gas annealing step, it is preferable to cool the α-sialon phosphor after the annealing step to about room temperature, and then heat-treat it in a hydrogen gas atmosphere. By performing the annealing step and the hydrogen gas annealing step consecutively, the fluorescent properties are significantly improved.

[0055] According to the inventors' findings, the hydrogen gas annealing process is a treatment for reducing defects in the phosphor. It is believed that the heat treatment in a hydrogen gas atmosphere allows hydrogen gas to penetrate into the crystal, stabilizing the crystal defects. As a result, it is believed that an α-sialon phosphor with an average linear expansion coefficient α' of 4.2 ppm / °C or more and 4.6 ppm / °C or less and with good luminescence characteristics can be obtained.

[0056] The heating temperature in the hydrogen gas annealing step is preferably 1300 to 1600°C, and more preferably 1400 to 1500°C. If the heating temperature is below 1300°C, the hydrogen gas will not penetrate into the crystal lattice, making it difficult to obtain the desired effect, while if it is above 1600°C, the crystal structure of the α-sialon phosphor may decompose. In addition, the heating temperature in the hydrogen gas annealing step is preferably set to a temperature lower than the heating temperature in the firing step.

[0057] The pressure in the hydrogen gas annealing step is preferably atmospheric pressure or near atmospheric pressure, specifically 0.02 to 0.9 MPa (gauge pressure). The time for the hydrogen gas annealing step is preferably 3 to 16 hours, more preferably 5 to 12 hours.

[0058] The purity of the hydrogen gas used in the hydrogen gas annealing step is preferably 99% or more. In particular, hydrogen gas with a purity of 99.9% or more is preferred. However, as long as the α-sialon phosphor of this embodiment can be obtained, a mixed gas of hydrogen gas and other gases may be used in the hydrogen gas annealing step. Examples of other gases include nitrogen gas and rare gases such as argon gas. The mixed gas preferably contains 30 vol% or more of hydrogen gas, and more preferably 40 vol% or more.

[0059] In this embodiment, it is preferable to perform an acid treatment after carrying out the above-described steps. This may reduce heterogeneous phases that do not contribute to light emission or that may cause deterioration of light emission characteristics, thereby further improving the light emission characteristics.

[0060] In the acid treatment step, for example, the α-sialon phosphor is immersed in an acidic aqueous solution. Examples of the acidic aqueous solution include an acidic aqueous solution containing one acid selected from acids such as hydrofluoric acid, nitric acid, and hydrochloric acid, and a mixed acid aqueous solution obtained by mixing two or more of the above acids. Among these, a hydrofluoric acid aqueous solution containing only hydrofluoric acid and a mixed acid aqueous solution obtained by mixing hydrofluoric acid and nitric acid are more preferred. The concentration of the stock solution of the acidic aqueous solution is appropriately set depending on the strength of the acid used, but is preferably 0.7% to 100%, and more preferably 0.7% to 40%. Furthermore, the temperature during the acid treatment is preferably 60°C to 90°C, and the reaction time (immersion time) is preferably 15 to 80 minutes.

[0061] High-speed stirring facilitates sufficient acid treatment of the phosphor surface. Here, "high speed" refers to a stirring speed of, for example, 400 rpm or higher when a laboratory-level magnetic stirrer is used, and more practically, a stirring speed of 400 rpm to 500 rpm. For the normal purpose of stirring, which is to constantly supply fresh acid to the particle surface, a stirring speed of about 200 rpm is sufficient. However, high-speed stirring at 400 rpm or higher facilitates sufficient treatment of the particle surface through physical action in addition to chemical action.

[0062] 1 is a schematic cross-sectional view illustrating the structure of a light emitting device 100. As shown in FIG. 1, the light emitting device 100 includes a light emitting element 120, a heat sink 130, a case 140, a first lead frame 150, a second lead frame 160, bonding wires 170 and 172, and a composite 40.

[0063] The light emitting element 120 is mounted in a predetermined region on the upper surface of the heat sink 130. Mounting the light emitting element 120 on the heat sink 130 can improve the heat dissipation properties of the light emitting element 120. Note that a packaging substrate may be used instead of the heat sink 130.

[0064] The light-emitting element 120 is a semiconductor element that emits excitation light. For example, an LED chip that emits light with a wavelength of 300 nm or more and 500 nm or less, which corresponds to near-ultraviolet to blue light, can be used as the light-emitting element 120. One electrode (not shown) disposed on the upper surface of the light-emitting element 120 is connected to the surface of the first lead frame 150 via a bonding wire 170 such as a gold wire. The other electrode (not shown) formed on the upper surface of the light-emitting element 120 is connected to the surface of the second lead frame 160 via a bonding wire 172 such as a gold wire.

[0065] A generally funnel-shaped recess whose diameter gradually increases from the bottom to the top is formed in the case 140. The light emitting element 120 is provided on the bottom of the recess. The wall of the recess surrounding the light emitting element 120 serves as a reflector.

[0066] The composite 40 is filled in the recess whose wall surface is formed by the case 140. The composite 40 is a wavelength conversion member that lengthens the wavelength of the excitation light emitted from the light emitting element 120. The composite of this embodiment is used as the composite 40, and the phosphor 1 of this embodiment is dispersed in a sealing material 30 such as a resin. The light emitting device 100 emits a mixed color of the light from the light emitting element 120 and the light generated from the phosphor 1 that is excited by absorbing the light from the light emitting element 120. It is preferable that the light emitting device 100 emits white light by mixing the light from the light emitting element 120 and the light generated from the phosphor 1.

[0067] Incidentally, examples of resins that can be used for the sealing material 30 in the composite 40 include transparent resins such as silicone resin, epoxy resin, and urethane resin. The composite 40 can be produced, for example, by adding the α-sialon phosphor of this embodiment to a liquid resin or powdered glass or ceramics, mixing them uniformly, and then curing or sintering them by heat treatment.

[0068] The light emitting device 100 of this embodiment has good light emitting characteristics because it uses the above-mentioned α-sialon phosphor as the phosphor 1 .

[0069] Incidentally, although FIG. 1 illustrates a surface-mounted light-emitting device, the light-emitting device is not limited to the surface-mounted type, and may be a bullet type, a COB (chip-on-board) type, or a CSP (chip-scale package) type.

[0070] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various other configurations may be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of achieving the object of the present invention are included in the present invention.

[0071] The embodiments of the present invention will be described in detail based on Examples and Comparative Examples. However, it should be noted that the present invention is not limited to the Examples.

[0072] Example 1: Production of α-sialon phosphor In a glove box, the raw material powder was mixed with Si to obtain a compound composition such that the m value was 3.75, the n value was 0, the x value was 1.795, and the y value was 0.08. 3 N 4 powder (manufactured by Ube Industries, Ltd., E10 grade) 60.14 mass%, AlN powder (manufactured by Tokuyama Corporation, E grade) 23.96 mass%, EuN powder (manufactured by Kojundo Chemical Laboratory Co., Ltd.) 2.07 mass%, and Ca 3 N 2 The mixture was dry-blended with 13.83% by mass of a powder (manufactured by Kojundo Chemical Research Institute) and then passed through a nylon sieve with a mesh size of 250 μm. A raw material mixed powder was thus obtained. 120 g of this raw material mixed powder was filled into a cylindrical boron nitride container (manufactured by Denka Co., Ltd., N-1 grade) with a lid and an internal volume of 0.4 liters.

[0073] The container filled with the raw material mixed powder was heat-treated in an electric furnace equipped with a carbon heater in a nitrogen atmosphere at atmospheric pressure at 1800°C for 16 hours. Because calcium nitride contained in the raw material mixed powder is easily hydrolyzed in air, the boron nitride container filled with the raw material mixed powder was removed from the glove box, quickly placed in the electric furnace, and immediately evacuated to a vacuum to prevent reaction of the calcium nitride.

[0074] The synthesized product was lightly crushed in a mortar and passed through a sieve with 150 μm openings to obtain a phosphor powder. When the crystalline phase of this phosphor powder was examined by powder X-ray diffraction measurement (hereinafter referred to as XRD measurement) using CuKα radiation, the crystalline phase present was found to be α-sialon.

[0075] The boron nitride container filled with the obtained phosphor powder was heat-treated in an electric furnace equipped with a carbon heater in a nitrogen atmosphere at atmospheric pressure at 1400°C for 16 hours (annealing process). The composite was lightly crushed in a mortar and passed through a sieve with 150 μm openings to obtain phosphor powder. Thereafter, the boron nitride container filled with the phosphor powder was heat-treated in an electric furnace equipped with a metal heater in a hydrogen atmosphere at atmospheric pressure at 1400°C for 16 hours (hydrogen annealing process). The composite was lightly crushed in a mortar and passed through a sieve with 150 μm openings to obtain phosphor powder.

[0076] Next, 50 ml of 50% hydrofluoric acid and 50 ml of 70% nitric acid were mixed to prepare a mixed solution. 300 ml of distilled water was added to the mixed solution to dilute the concentration of the mixed solution to 25%, preparing 400 ml of mixed acid aqueous solution. 30 g of the powder consisting of the above-mentioned α-sialon phosphor particles was added to this mixed acid aqueous solution, and acid treatment was performed by immersing the mixed acid aqueous solution for 60 minutes while maintaining the temperature of the mixed acid aqueous solution at 80°C and stirring it at a rotation speed of 450 rpm using a magnetic stirrer. After the acid treatment, the powder was thoroughly washed with distilled water to remove the acid, filtered, dried, and then passed through a sieve with 45 μm openings. This resulted in a powdered α-sialon phosphor.

[0077] The composition of the obtained α-sialon phosphor was analyzed to determine x, y, x+y, m, and n in the general formula. The specific method of composition analysis is as follows.

[0078] The Eu, Ca, Si, and Al contents in the phosphor were quantitatively analyzed using an ICP optical emission spectrometer (SPECTRO Corporation, CIROS-120) after dissolving the α-sialon phosphor by pressure acid decomposition. The O and N contents in the phosphor were quantitatively analyzed using an oxygen and nitrogen analyzer (HORIBA Ltd., EMGA-920). The composition analysis results were calculated based on the general formula (Ca, x , Eu y ) (Si 12-(m+n) Al m+n ) (O n N 16-n ), the m value was 3.5, the n value was 0.27, the x value was 1.63, the y value was 0.05, and the x+y value was 1.68.

[0079] <Calculation of lattice constant and average linear expansion coefficient> (X-ray diffraction measurement) An α-sialon phosphor was placed on a sample plate, and the sample was spread out with a glass plate so that the sample surface was flush with the surface of the sample plate. X-ray diffraction measurement was then performed under the following conditions. Si (NIST SRM 640c, hereinafter also referred to as "Si_640c") was also measured as an angle standard sample (external standard). Equipment: Rigaku X-ray diffractometer Ultima IV; Optical system: Parallel beam method; X-ray source: Cu sealed tube; Applied voltage / current: 40 kV / 40 mA; Detector: Scintillation counter; Measurement stage: High temperature sample device; Measurement atmosphere: N 2 Flow (30 mL / min) Set temperature 25°C, 300°C, 500°C, 700°C, 900°C (other than Si_640c) 25°C (Si_640c) Heating rate 20°C / min Interval 10 min Measurement angle range 2θ = 24 to 140° Sampling width 0.04° Scan speed 2° / min Repeated measurements 4 times (other than Si_640c) 3 times (Si_640c) Slit configuration Incident side solar slit: 5.0°, receiving side solar slit: 5.0° Thin film PSA DS: 1 mm, DS vertical: 10 mm, SS: open, RS: open Sample plate Made of Pt

[0080] (Calculation of Lattice Constant) In the above X-ray diffraction measurement, the measurement results at each temperature (25°C, 300°C, 500°C, 700°C, 900°C) were used to perform analysis using powder X-ray diffraction pattern comprehensive analysis software Jade 9 manufactured by Materials Data. This allowed for precise calculation of the lattice constant. The conditions for the analysis are described below. Method: Pawley method Analysis temperatures: 25°C, 300°C, 500°C, 700°C, 900°C Angle range: 2θ = 24 to 140° (Note 1) Background: 4th-Order Polynomial Refinement Peak shift: Zero-point correction 2θ: 0.005948 (Note 2) Sample displacement cos θ: 0 (fixed) Vertical divergence cot(2θ): -0.012557 (Note 2) Peak shape: Pseudo-Voigt function Peak intensity ratio: Refinement (Note 1: In analysis by the Pawley method over the angle range 2θ = 24 to 140°, if diffraction lines other than those of α-sialon appear, these diffraction lines were appropriately excluded from the analysis.) (Note 2: The measurement results of a standard sample (Si_640c) were analyzed and the obtained value was used.)

[0081] (Calculation of volume expansion coefficient) (1) Calculate the lattice constant a T and c T A graph was created by plotting the above. An approximate linear equation was then determined for the range from 25 to 900°C. The approximate linear equation can be determined by the least squares method. Incidentally, in the crystal structure of α-sialon, T and b T (2) Using the approximate linear equation, the lattice constant a at 25°C 25 and c 25 (3) Using the approximate linear equation, the lattice constant a at 900°C was calculated. 900 and c 900 (4) Lattice constant a 25 and c 25 Using the value of 25 (Note 3) (5) Lattice constant a 900 and c 900 Using the value of , the lattice volume V at 900 ° C. 900(Note 3) (6) The volume expansion coefficient β was calculated using the following formula. Here, ΔT is 900°C - 25°C = 875°C. (Note 3: The crystal structure of α-sialon is hexagonal.)

[0082]

[0083] (Calculation of average linear expansion coefficient) The average linear expansion coefficient α' was calculated using the formula α' = β / 3. This formula α' = β / 3 is used to calculate the average linear expansion coefficient of a polycrystalline body, assuming that the sample is an isotropic material.

[0084] (Average linear expansion coefficient α at 25 to 300°C 1 ' and the average linear expansion coefficient α at 700 to 900°C 2 Calculation of the average linear expansion coefficient α at 25 to 300°C by the above-mentioned series of procedures. 1 ' and the average linear expansion coefficient α at 700 to 900°C 2 ´ was calculated.

[0085] (Measurement of particle size distribution and calculation of median diameter) Using a Microtrac MT3300EX II (Microtrac Bell Corporation), measurements were made by a laser diffraction scattering method in accordance with JIS R1629:1997. Specifically, first, 0.5 g of powdered α-sialon phosphor was added to 100 cc of ion-exchanged water, and a dispersion treatment was carried out for 3 minutes using an Ultrasonic Homogenizer US-150E (Nihon Seiki Seisakusho Co., Ltd., tip size φ20 mm, amplitude 100%, oscillation frequency 19.5 kHz, amplitude approximately 31 μm), to obtain a dispersion. This dispersion was set in the MT3300EX II, and the particle size distribution was measured. The median diameter D50 was calculated from the obtained particle size distribution.

[0086] <Evaluation of Light-Emitting Properties> The absorptance, internal quantum efficiency, and external quantum efficiency of the obtained powdered α-sialon phosphor were measured using a spectrophotometer (MCPD-7000, manufactured by Otsuka Electronics Co., Ltd.) and calculated using the following procedure. The powdered α-sialon phosphor was filled into a concave cell so that the surface was smooth. This cell was attached to a predetermined position on an integrating sphere. Monochromatic light, separated into wavelengths of 455 nm from a light source (Xe lamp), was introduced into the integrating sphere using an optical fiber. This monochromatic light was irradiated onto a phosphor sample, and the fluorescence spectrum of the sample was measured. A standard reflector (Spectralon, manufactured by Labsphere) with a reflectance of 99% was attached to the sample, and the spectrum of excitation light with a wavelength of 455 nm was measured. At this time, the number of excitation light photons (Qex) was calculated from the spectrum in the wavelength range of 450 nm to 465 nm. A cell filled with powdered α-sialon phosphor was attached to the sample section, and the number of reflected excitation light photons (Qref) and the number of fluorescent photons (Qem) were calculated from the obtained spectral data. The number of reflected excitation light photons was calculated over the same wavelength range as the number of excitation light photons, and the number of fluorescent photons was calculated over the range of 465 nm to 800 nm. Absorption (%) = (Qex - Qref) / Qex x 100 Internal quantum efficiency (%) = (Qem / (Qex - Qref)) x 100 External quantum efficiency (%) = (Qem / Qex) x 100 When the standard sample NSG1301 sold by Sialon Corporation was measured using the above measurement method, the external quantum efficiency was 55.6% and the internal quantum efficiency was 74.8%. This sample was used as the standard to calibrate the instrument.

[0087] Example 2: Production and evaluation of α-sialon phosphor An α-sialon phosphor was produced in the same manner as in Example 1, except that the starting composition was changed. Then, the light-emitting properties were evaluated. The produced α-sialon phosphor had an m value of 3.0, an n value of 0.25, an x ​​value of 1.45, a y value of 0.05, and an x+y value of 1.50.

[0088] Example 3: Production and evaluation of α-sialon phosphor An α-sialon phosphor was produced in the same manner as in Example 1, except that the starting composition was changed. Then, the light-emitting properties were evaluated. The produced α-sialon phosphor had an m value of 4.0, an n value of 0.21, an x ​​value of 1.94, a y value of 0.06, and an x+y value of 2.01.

[0089] <Comparative Example 1: Production and Evaluation of α-SiAlON Phosphor> An α-SiAlON phosphor was produced in the same manner as in Example 1, except that the starting composition was changed and the hydrogen annealing step was not performed. Then, the light-emitting properties were evaluated. The produced α-SiAlON phosphor had an m value of 2.0, an n value of 0.32, an x ​​value of 0.94, a y value of 0.06, and an x+y value of 1.00.

[0090] Comparative Example 2: Production and Evaluation of α-SiAlON Phosphor An α-SiAlON phosphor was produced in the same manner as in Example 1, except that the starting composition was changed and the hydrogen annealing step was not performed. The luminescence characteristics were then evaluated. The produced α-SiAlON phosphor had an m value of 3.5, an n value of 1.47, an x ​​value of 1.70, a y value of 0.05, and an x+y value of 1.75.

[0091] The information on each example and comparative example is summarized in the table below. In the table, the units of each value are as follows: α', α 1 ´ and α 2 ´: ppm / °C a 25 and c 25 :Å V 25 :Å 3 Absorption rate, internal quantum efficiency and external quantum efficiency: %

[0092]

[0093]

[0094] As shown in Tables 1 and 2, the general formula: (Ca x , Eu y ) (Si 12-(m+n) Al m+n ) (O n N 16-n) α-sialon phosphors having a composition that satisfies the conditions 0<x<2.0, 0<y≦0.5, 0.3≦x+y≦2.2, 0<m≦4.0, and 0<n≦3.0, and having an average linear expansion coefficient α' of 4.2 ppm / °C or more and 4.6 ppm / °C or less at 25 to 900°C, exhibited better internal quantum efficiency and external quantum efficiency than α-sialon phosphors that did not meet these conditions.

[0095] This application claims priority based on Japanese Patent Application No. 2023-059122, filed on March 31, 2023, the disclosure of which is incorporated herein by reference in its entirety.

[0096] REFERENCE SIGNS LIST 1 Phosphor 30 Sealant 40 Composite 100 Light emitting device 120 Light emitting element 130 Heat sink 140 Case 150 First lead frame 160 Second lead frame 170 Bonding wire 172 Bonding wire

Claims

1. An α-type SiAlON phosphor represented by the following general formula, having an average linear expansion coefficient α' of 4.2 ppm / °C or more and 4.6 ppm / °C or less at 25 to 900°C. General formula: (Ca x , Eu y ) (Si 12-(m+n) A m+n ) (O n N 16-n In the above general formula, x, y, m and n satisfy the following: 0<x<2.0 0<y≦0.5 0.3≦x+y≦2.0 0<m≦4.0 0<n≦3.0 2. The α-sialon phosphor according to claim 1, wherein m satisfies 2.5≦m≦4.0 and 0<n≦0.

5.

3. The α-SiAlON phosphor according to claim 1 or 2, wherein the average linear expansion coefficient at 25 to 300°C is α 1 ', and the average linear expansion coefficient at 700 to 900°C is α 2 ´, then α 2 ´ / α 1 An α-sialon phosphor in which ' is 1.3 to 1.

8.

4. The α-SiAlON phosphor according to claim 1 or 2, wherein the lattice constant a of the unit lattice is less than 25° C. 25 is 7.900 Å or more and 7.960 Å or less, and the lattice constant c 25 The α-sialon phosphor has a surface roughness of 5.720 Å or more and 5.780 Å or less.

5. The α-SiAlON phosphor according to claim 1 or 2, wherein the lattice volume V of the unit lattice at 25° C. 25 is 308 Å 3 More than 320 Å 3 The α-SiAlON phosphor is shown below.

6. An α-sialon phosphor according to claim 1 or 2, wherein in the general formula, x, y, m and n satisfy the following: 1.3≦x<2.0 0.01≦y≦0.1 1.3≦x+y≦2.0 2.8≦m<4.0 0.1≦n≦0.27 7. A light emitting device comprising: a light emitting element; and a wavelength conversion section which contains the α-sialon phosphor according to claim 1 or 2 and converts the wavelength of light emitted from the light emitting element into a longer wavelength.

Citation Information

Patent Citations

  • High-lighting-effect and high-stability alpha-SiAlON:Eu&lt;2+&gt; yellow fluorescent powder and preparation method thereof

    CN107057696A

  • Ca-CONTAINING α-SIALON PHOSPHOR AND METHOD FOR PRODUCING THE SAME

    JP2012224757A

  • Method for producing powdered precursor material, powdered precursor material and use thereof

    JP2016506976A

  • Oxynitride fluorescent substance powder, silicon nitride powder for manufacturing same, and method for manufacturing same

    WO2013054901A1

  • Oxynitride phosphor powder

    WO2013147066A1