Tungsten wire

By controlling the crystal orientation in rhenium-tungsten alloy wires, specifically within 15° from <101> parallel to the wire drawing direction, the breakage of tungsten wires during drawing is minimized, improving yield and workability for medical needle production.

WO2024204092A1PCT designated stage expired Publication Date: 2024-10-03NITERRA MATERIALS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011753
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-25
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

The challenge is to reduce breakage of tungsten wires during drawing, particularly for thin wires with diameters of 0.05 mm to 0.3 mm, which affects the yield and increases man-hours due to frequent disconnections and cracks, and existing methods do not effectively control crystal orientation near the finished size.

Method used

A tungsten wire made from a rhenium-tungsten alloy with controlled crystal orientation, where EBSD analysis shows a specific crystal orientation distribution within 15° from <101> parallel to the wire drawing direction, ensuring a high area ratio of 90% to 99.9% in the central area and 70% to 93% in the peripheral area, along with optimized processing conditions for heat treatment and wire drawing.

Benefits of technology

This approach significantly reduces wire breakage during drawing, enabling longer wire lengths and improved yield by ensuring uniform crystal orientation and reduced brittleness, thus enhancing the workability and strength of the wire for medical needle applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011753_03102024_PF_FP_ABST
    Figure JP2024011753_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a tungsten wire in which breakage during wire drawing, particularly when approaching a finished size having a diameter of 0.05-0.3 mm, by controlling the crystal alignment. The tungsten wire is composed of a tungsten alloy containing rhenium. When an EBSD analysis is performed on sections of the body of the tungsten wire having a unit area of 40 μm × 40 μm at concentric positions within 100 μm from the center axis in a radial cross section of the wire perpendicular to the wire-drawing direction, the proportion of the area ratio, on an IPF map, occupied by crystal orientations having an orientation difference within 15° from the <101> plane parallel to the wire-drawing direction is 90-99.9% in the field of view of measurement.
Need to check novelty before this filing date? Find Prior Art

Description

Tungsten wire

[0001] An embodiment of the present invention relates to a tungsten wire.

[0002] Traditionally, stainless steel needles have been commonly used as medical suture needles, but in recent years, there has been a growing need for thinner medical needles to reduce the burden on patients. However, as needles become thinner, they tend to bend and warp more easily, resulting in a decrease in workability within a short period of time. To prevent this, a material with higher strength and rigidity than stainless steel is required. In particular, rhenium-tungsten alloys (Re-W alloys) are materials with high strength and rigidity due to the strengthening of the solid solution of rhenium in tungsten.

[0003] In recent years, with the advancement of mass production of suture needles, when using rhenium-tungsten wire (ReW wire), long wire is required for automatic and continuous processing into a desired needle shape. To obtain such thin-diameter ReW wire, a sintered body is first subjected to primary processing such as rolling and wiredrawing (wire drawing) to process it into a diameter of 0.3 mm to 1.2 mm (medium wire) or 0.05 mm to 0.3 mm (thin wire). Hereinafter, a diameter of 0.3 mm to 1.2 mm may be referred to as a medium wire, and a diameter less than 0.3 mm may be referred to as a thin wire. Subsequently, an appropriate amount of thin ReW wire is subjected to additional necessary processes such as wiredrawing and heat treatment to achieve the desired diameter. During this thinning process, cracks and breaks originating from cracks are likely to occur during the wiredrawing process. Breaks during the wiredrawing process of thin wire make it impossible to obtain the required length using a multi-stage wiredrawing machine that processes with multiple dies, significantly reducing yield. Even if the required length can be secured, repairing and restarting the line after a breakage will increase the number of man-hours required.

[0004] Conventional countermeasures against wire breakage include strict control of lubricant management and wire drawing conditions. For example, the lubricant applied to the surface of a tungsten wire contains graphite (C) powder and a thickener, and has a specific gravity of 1.0 g / cm. 3 1.1g / cm or more 3 The change in specific gravity during processing is 0.05 g / cm or less. 3The wire drawing process is performed by controlling the tungsten wire temperature to be 500°C or higher and 1300°C or lower, the wire drawing die temperature to be 300°C or higher and 650°C or lower, the wire drawing speed to be 10 m / min or higher and 70 m / min or lower, and the area reduction rate in the final wire drawing step to be 5% or higher and 15% or lower (see Patent Document 1).

[0005] In addition, there are some products that improve workability by controlling the number of recrystallizations through heat treatment in the intermediate process. For example, when the cross-sectional area reduction rate (area reduction rate) of the molded product from the sintered compact exceeds 75% and reaches 90% or less, a final recrystallization treatment is carried out to reduce the number of recrystallized grains in the center and surface layer of the molded product to 500 grains / mm. 2 More than 800 pieces / mm 2 There are ReW wires that are adjusted as follows (see Patent Document 2). Patent Document 1 describes a method of suppressing fluctuations in workability by limiting the processing conditions in the wiredrawing process. Patent Document 2 describes a method of applying a predetermined area reduction rate from the sintered body to the recrystallization process and controlling the number of crystals by heat treatment, and describes the effect of processing up to a finished diameter of 1.0 mm.

[0006] International Publication No. 2009 / 066659 Japanese Patent Application Laid-Open No. 3-219039 International Publication No. 2023 / 008430

[0007] The problem to be solved by the present invention is to provide a tungsten wire that improves cutting during wire drawing, particularly in the vicinity of the finished size of a diameter of 0.05 mm or more and 0.3 mm or less, indicated by the symbol φ, by controlling the crystal orientation.

[0008] In order to solve the above problems, the tungsten wire according to the embodiment is a tungsten wire made of a tungsten alloy containing rhenium (Re), and when EBSD analysis is performed on a unit area of ​​40 μm × 40 μm at a position concentrically within 100 μm from the central axis in a wire radial cross section perpendicular to the wiredrawing direction of a main body of the tungsten wire, the proportion of the area ratio occupied by crystal orientations within an orientation difference of 15° from <101> parallel to the wiredrawing direction on an IPF map (Inverse Pole Figure map) is 90% or more and 99.9% or less within the measurement field of view.

[0009] 1 is a perspective view showing an example of a sample taken from a ReW wire according to an embodiment; a schematic diagram showing a schematic explanation of crystal orientation; a schematic diagram showing a schematic explanation of a bcc structure; and a schematic diagram showing a schematic explanation of deformation in a die during wire drawing and stress acting on the center and surface.

[0010] Hereinafter, a tungsten wire according to an embodiment will be described with reference to the drawings. Hereinafter, the tungsten wire will be referred to as a ReW wire. Note that the drawings are schematic, and the dimensional ratios of the various parts are not limited to those shown in the drawings.

[0011] Fig. 1 shows an example of a sample taken from the ReW line of the embodiment. In Fig. 1, the axial direction of the sample is defined as the ND (Normal Direction). The cross section perpendicular to the axial direction of the sample is defined as the measurement surface S of the sample. 0 The horizontal (radial) direction in a cross section perpendicular to the axial direction of the sample is defined as the transverse direction (TD). The horizontal (radial) direction in a cross section perpendicular to the axial direction of the sample, and perpendicular to the TD, is defined as the reference direction (RD). While the sampling location is arbitrary, it is recommended to sample at least one position (n = 1) at each of the front and rear ends of a single ReW wire, in order to ensure high yield in subsequent processes and to check for variations over the entire length. The front and rear ends are not included in the sampling because they have unstable conditions due to the start and stop of the wiredrawing equipment. The length of the unstable portion varies depending on the layout and size of the equipment. The length of the sample taken from the ReW wire is preferably a length (100 mm to 150 mm) that allows multiple cross-sectional observations by embedding them in resin. After wiredrawing, the ReW wire has a mixture layer on its surface. This mixture layer contains W, C, and O as constituent elements. The main body portion excluding this mixture layer is used as the sample. The sample was cut in a cross section (S) perpendicular to the axial direction (ND (Normal Direction)). 0 ) is filled with resin and polished to form a measurement surface. Etching is performed as necessary. The surface roughness Ra of the measurement surface is measured with a laser microscope at 50x magnification, and the surface roughness Ra is 0.08 μm or more and 0.12 μm or less. The mixture layer can be removed by surface polishing, for example, by electrolysis.

[0012] Measurement surface S in FIG. 0 In contrast, the EBSD (Electron Backscattered Diffraction) method is used to analyze the crystal orientation. EBSD involves irradiating a crystalline sample with an electron beam. The electrons are diffracted and emitted from the sample as reflected electrons. This diffraction pattern is projected, and the crystal orientation can be measured from the projected pattern. X-ray diffraction (XRD) is a method for measuring the average value of the crystal orientation of multiple crystals. In contrast, EBSD can obtain information on each crystal grain and measure the crystal orientation. The crystal orientation data can then be used to analyze the orientation distribution of the crystal grains. This method is also called the EBSP (Electron Backscattered Diffraction Pattern) method.

[0013] For EBSD analysis, for example, a thermal field emission scanning electron microscope (TFE-SEM) JSM-7800F Prime manufactured by JEOL Ltd. and a DigiViewIV slow scan CCD camera, OIM Data Collection ver. 7.3x, and OIM Analysis ver. 8.0 manufactured by TSL Solutions Co., Ltd. can be used.

[0014] The EBSD analysis was performed by observing three locations at 1000x magnification within 100 μm of the sample's central axis (center) and within 50 μm of the sample's outer periphery (outer periphery). The crystal orientations at these three locations were determined, and the area ratios were then calculated. The average of the area ratios of the crystal orientations at these three locations was then calculated. Each measurement area was 40 μm x 40 μm. The measurement areas may overlap. Alternatively, the average of the area ratios of the crystal orientations measured 16 times in a 10 μm x 10 μm area at a magnification of 5000x may be calculated, with the average being calculated as one measurement of a 40 μm x 40 μm area. Therefore, for example, if a 10 μm x 10 μm area is used as a single measurement area, 16 x 3 (48) measurements may be performed without overlapping, and the area ratios of the crystal orientations may be calculated for each measurement area to calculate the average of the 48 measurements. Furthermore, if the sample is a thin ReW wire (e.g., 30 μm in diameter), the crystal orientations at the center of multiple cross sections may be measured and the area ratios of the crystal orientations determined may be averaged. The magnification is preferably 1000x or greater. If the magnification is less than 1000x, the spatial resolution may be reduced, potentially preventing measurements with sufficient accuracy. The measurement conditions are an electron beam acceleration voltage of 15 kV, a probe current of 15 nA, a sample tilt angle of 70 degrees, and an interval of 200 nm / step. Here, the sample is the main body of the ReW wire excluding the mixture layer. The ReW wire of the embodiment may be one that does not substantially contain a mixture layer on the surface, one that is essentially composed of Re, W, and inevitable impurities (e.g., oxygen atoms), or one that contains a mixture layer on the surface. Even when the ReW wire of the embodiment has a mixture layer on the surface, when EBSD analysis is performed on the center of the main body portion excluding the mixture layer, the area ratio of crystal orientations within an orientation difference of 15° from <101> parallel to the wiredrawing direction on the IPF map is 90% or more and 99.9% or less within the measurement field of view.

[0015] An IPF map (Inverse Pole Figure map) is a crystal orientation map based on an inverse pole figure. It can show the distribution of specified crystal orientations and orientation ranges facing a specified sample direction (ND, TD, RD, etc.). In addition, image analysis can be used to determine the area ratio of specified crystal orientations and orientation ranges. IPF maps are created in accordance with the EBSD measurement method described above.

[0016] Crystal orientations are indicated by using fundamental vectors. A notation consisting of a combination of square brackets and numbers enclosed within square brackets ([ ]) indicates only a specific crystal orientation. A notation consisting of a combination of angle brackets and numbers enclosed within angle brackets (< >) indicates a specific crystal orientation and its equivalent direction. For example, <101> indicates that it includes a direction equivalent to

[101] . Also, for example, the preferred orientation being <101> indicates that the <101> orientation is the most prevalent of all crystal orientations.

[0017] Each metal crystal lattice has its own specific slip plane and slip direction. From a microscopic perspective, plastic deformation occurs due to the slip of the crystal lattice. Repeated deformation in the same direction, such as in wire drawing, eventually converges to a specific slip plane and slip direction. It is known that in body-centered cubic (bcc) metals, wire drawing generates a <110> orientation texture parallel to the wire drawing direction (this becomes the final stable orientation). Figure 2 shows an overview of the

[110] and

[101] orientations, and Figure 3 shows an overview of the atomic arrangement of bcc. As can be seen from the figure, <101> and <110> are equivalent in bcc.

[0018] In the ReW wire of the embodiment, the area ratio of the crystal orientation within 15° of the <101> parallel to the ND in the center is 90% to 99.9% in the measurement field of view. The misorientation refers to the relative difference in the orientation of the crystal grains. In the center, the area ratio of the crystal orientation within 15° of the <101> parallel to the ND is preferably 95% to 99.9%, more preferably 98% to 99.9%. Furthermore, the area ratio of the crystal orientation within 5° of the <101> is preferably 88% to 98%, more preferably 92% to 98% in the measurement field of view. The ReW wire of the embodiment has a bcc structure, and as the wiredrawing process proceeds, it converges to the <101> parallel to the ND. When the proportion of crystal orientations within 15° of <101> exceeds 99.9% and when the proportion of crystal orientations within 5° of <101> exceeds 98%, plastic deformation during thin wire processing becomes difficult, and cracks become more likely to occur. Alternatively, recrystallization annealing becomes necessary at the stage of thin wire processing when the diameter is large. Recrystallization reduces the workability of ReW wire and makes it more likely to crack. When the proportion of crystal orientations within 15° of <101> is less than 95% and when the proportion of crystal orientations within 5° of <101> is less than 88%, strengthening by processing to compensate for the brittleness of the W material becomes insufficient, and cracks become more likely to occur during wire drawing from the center line.

[0019] Figure 4 shows the deformation in the die during wire drawing and the stress acting on the center 2 and surface 1 (also called the outer periphery 1). In the ReW wire for wire drawing, tensile stress acting on the ND at the center advances plastic deformation, and the <101> orientation becomes the preferred orientation. In the outer periphery 1, deformation due to shear force is applied, so the preferred orientation is <101>, but the proportion of the <227> orientation increases.

[0020] In the ReW wire of the embodiment, the area ratio of the crystal orientation within 15° of the <101> orientation parallel to the ND in the outer periphery is preferably 70% to 93% within the measurement field of view, and more preferably 85% to 93%. Furthermore, the area ratio of the crystal orientation within 15° of the <227> orientation parallel to the ND is preferably 20% or less within the measurement field of view. If the ratio of the crystal orientation within 15° of the <101> orientation is less than 70%, or even if the ratio of the crystal orientation within 15° of the <227> orientation is more than 20%, it is possible that a large shear force was applied to the ReW wire, and the wiredrawing conditions were abnormal (such as abnormal lubrication). In such cases, cracks are likely to occur. Furthermore, the large shear force causes a difference in residual stress between the inside and outside, which may cause cracks. The upper limit of the proportion of crystal orientations within 15° of the <101> parallel to the ND is preferably 93% or less to maintain a balance with the interior of the ReW wire for wire drawing. If it exceeds 93%, there is a possibility that only the outer periphery has been processed. There is no particular limit to the lower limit of the proportion of the area ratio occupied by crystal orientations within 15° of the <227> parallel to the ND in the outer periphery, but since the outer periphery is subjected to shearing force by the die, 3% or more is preferred. A more preferred lower limit is 5%.

[0021] The grain size is determined by creating a crystal grain map using the EBSD analysis data. When there are two or more consecutive measurement points with a crystal orientation angle difference of 5° or less, the crystal grains are identified as the same grain and color-mapped. Next, for each crystal grain identified in the crystal grain map, the diameter of a circle with the same area (circle equivalent diameter) is calculated and plotted as a histogram. The average grain size (d A ) is the total number of grains N A , the area ratio of each grain is A i , the equivalent circle diameter is d i When this is the case, it can be calculated using the following formula:

[0022]

[0023] In the embodiment, the ReW wire has an average grain size of 0.15 μm or more and 0.23 μm or less on the grain map of the center. The preferred range of the average grain size is 0.17 μm or more and 0.21 μm or less. The maximum grain size is 0.8 μm or more and 2.0 μm or less. The preferred range of the maximum grain size is 1.0 μm or more and 1.8 μm or less. If the average grain size is less than 0.15 μm, grain boundary strengthening may increase the drawing force during fine wire processing, making cracks more likely to occur. If the average grain size exceeds 0.23 μm, the strengthening by processing to compensate for the brittleness of the W material may be insufficient, making cracks more likely to occur during wire drawing from the center line. Furthermore, the strength may be insufficient at the finished size, such as for medical needles. If the maximum grain size exceeds 2.0 μm, the presence of such grains may result in a heterogeneous structure, resulting in differences in strength and deformability in microregions, which may cause heterogeneity in internal stress and lead to cracks. There is no particular lower limit to the maximum particle size, but it is preferably 0.8 μm or more.

[0024] In the ReW wire of the embodiment, the ratio of the average grain size of the center portion to the average grain size of the outer periphery is greater than 1.00 and less than 1.20 on the crystal grain map of the center portion and the outer periphery. Here, when the average grain size of the center portion is d1 and the average grain size of the outer periphery is d2, this ratio is expressed as d1 / d2. A more preferable range of d1 / d2 is 1.02 or more and 1.15 or less. If the ratio is 1.20 or more, it is possible that only the outer periphery has been processed or that a large shear force has been applied, making cracks more likely to occur during thinning processing. If the ratio is 1.00 or less, it is possible that only the outer periphery has recrystallized due to heating during the processing step up to the midline. In such cases, there is a difference in deformability between the inside and outside, causing inhomogeneity in internal stress and causing cracks during the thinning process.

[0025] The ReW wire of the embodiment has an Re content of 11 wt% or more and 30 wt% or less. If the Re content is less than 11 wt%, the strength decreases, and when used in, for example, a medical suture needle, it will not be able to maintain the specified shape, resulting in a decrease in surgical precision. On the other hand, if the Re content exceeds 30 wt%, the deformation stress becomes too large, making it difficult to process into a thin wire. The Re content is a value obtained by analysis using inductively coupled plasma optical emission spectroscopy (ICP-OES).

[0026] Next, a method for manufacturing the ReW wire according to this embodiment will be described. The manufacturing method is not particularly limited, but the following method can be given as an example.

[0027] W powder and Re powder are mixed so that the Re content is 11 wt% or more and 30 wt% or less. While there are no particular limitations on the mixing method, a method in which the powders are made into a slurry using water or an alcohol-based solution and mixed is particularly preferred, as this produces a powder with good dispersibility. The Re powder to be mixed has, for example, an average particle size of less than 8 μm. The W powder is either pure W powder excluding unavoidable impurities, or doped W powder containing a K amount that takes into account the yield of the wire rod. The W powder has, for example, an average particle size of less than 16 μm.

[0028] Next, the mixed powder is placed in a mold and press-molded. The pressing pressure is preferably 150 MPa or higher. For ease of handling, the molded body may be pre-sintered in a hydrogen furnace at 1200°C to 1400°C. The resulting molded body is sintered in a hydrogen atmosphere, an inert gas atmosphere such as argon, or a vacuum. The sintering temperature is preferably 2500°C or higher. At temperatures below 2500°C, the diffusion of Re and W atoms during sintering is insufficient. The upper limit of the sintering temperature is 3400°C (below the melting point of W, 3422°C). If the upper limit of the sintering temperature exceeds the melting point of W (3422°C), the molded body may not maintain its shape and may become defective. The relative density after sintering is preferably 90% or higher. By achieving a relative density of 90% or higher, it is possible to reduce cracking, chipping, breakage, etc. during the subsequent swaging process.

[0029] Molding and sintering may be performed simultaneously by hot pressing in a hydrogen atmosphere, an inert gas atmosphere such as argon, or in a vacuum. The pressing pressure is preferably 100 MPa or more, and the heating temperature is preferably 1700°C to 2825°C. This hot pressing method can produce a dense sintered body even at a relatively low temperature.

[0030] The sintered body obtained in this sintering step is subjected to a first rolling and punching process (SW process). The first SW process is preferably carried out at a heating temperature of 1300°C or higher and 1600°C or lower. The reduction rate of the cross-sectional area (area reduction rate) in one heat treatment (one heat) is preferably 5% or higher and 15% or lower. After the first SW process, heat treatment is carried out to control the crystal orientation. Since the sintered body does not have a true density after the first SW process, strain in the sintered body is likely to become non-uniform. For this reason, non-uniformity is removed by heat treatment. Heat treatment can be carried out by direct resistance heating in a hydrogen atmosphere, for example. In the case of direct resistance heating, the current is 14 A / mm 2 More than 17A / mm 2 The current value is preferably 14 A / mm or less. 2 If the current is less than 17 A / mm, the strain relief in the first SW process will be insufficient. 2 If the strain exceeds this value, uneven strain will cause coarse recrystallization at the outer periphery of the cross section of the sintered body, making the structure uneven. This makes it difficult to control the crystal orientation.

[0031] After the first SW processing and heat treatment, rolling processing (RM (rolling machine) processing) is performed. RM processing is preferably performed at a heating temperature of 1200°C or higher and 1600°C or lower. The area reduction rate per heat is preferably 40% or higher and 75% or lower. As the rolling mill, a two-way roller rolling mill, a four-way roller rolling mill, a die roll rolling mill, or the like can be used. RM processing makes it possible to significantly improve manufacturing efficiency.

[0032] The sintered body (ReW bar) after RM is subjected to a second SW process. The second SW process is preferably performed at a heating temperature of 1200°C or higher and 1500°C or lower. The area reduction rate per heat is preferably about 5% or higher and 20% or lower.

[0033] The ReW bar material after the second SW process is then subjected to a recrystallization treatment. The recrystallization treatment is preferably performed, for example, using a high-frequency heating device in a hydrogen atmosphere, an inert gas atmosphere such as argon, or a vacuum, at a treatment temperature in the range of 1900°C to 2100°C. If the heat treatment temperature is below 1900°C, the recrystallization treatment is insufficient, and the processed structure and the recrystallized structure tend to be mixed. If the heat treatment temperature exceeds 2100°C, coarse recrystallization occurs, and the structure tends to become non-uniform. By performing the recrystallization treatment in the range of 1900°C to 2100°C, it is possible to control the crystal orientation.

[0034] The ReW bar that has completed the recrystallization treatment is subjected to a third SW process. The third SW process is preferably carried out at a heating temperature of 1200°C or higher and 1500°C or lower. The area reduction rate per heat is preferably about 10% or higher and 30% or lower. The third SW process is carried out until the ReW bar has a diameter that can be drawn (preferably a diameter of 2 mm or higher and 4 mm or lower).

[0035] The ReW bar material after the third SW process is subjected to the first wiredrawing process to a diameter of 0.3 mm to 1.2 mm. The first wiredrawing process is preferably performed in a temperature range of 600 ° C to 1100 ° C. In the ReW wire of the present invention, a sufficient oxide film must be formed on the tungsten surface to allow the carbon-based lubricant to penetrate the surface sufficiently during the wiredrawing process. Therefore, it is desirable to perform annealing treatment multiple times at 900 ° C to 1200 ° C in an oxidizing atmosphere while the diameter is 0.3 mm to 1.2 mm. Below 900 ° C, the oxide film is not sufficiently formed, the lubricating effect is insufficient, and the wire is prone to breakage. On the other hand, above 1200 ° C, the strength of the ReW wire itself decreases, leading to wire breakage during drawing, so the above temperature range is preferred.

[0036] The ReW wire that has undergone the first wiredrawing process is further subjected to a second wiredrawing process to a diameter of 0.05 mm to 0.3 mm. The second wiredrawing process is preferably performed at a temperature of 500°C to 800°C. The workable temperature varies depending on the wire diameter, with the larger the diameter, the higher the temperature. If the temperature is lower than the workable temperature, cracks and wire breakage occur frequently. If the temperature is higher than the workable temperature, seizure between the ReW wire and the die occurs, and the deformation resistance of the ReW wire decreases, causing fluctuations in the diameter after wiredrawing (thinning) due to the drawing force. The area reduction rate is preferably 15% to 35%. If it is less than 15%, differences in the internal and external structure and residual stress occur during the process, causing cracks. If it is greater than 35%, the drawing force becomes excessive, causing large fluctuations in the diameter after wiredrawing and resulting in breakage. The wiredrawing speed is determined by the balance between the capacity of the heating device, the distance from the device to the die, and the area reduction rate. Polishing may be performed during the wiredrawing process. The polishing process can be performed by electrochemical polishing (electrolytic polishing) in a sodium hydroxide solution with a concentration of 7 wt% to 15 wt%. Similarly, a heat treatment for strain relief (to prevent recrystallization) may be added. The wire is then drawn to produce a ReW wire with a diameter of 0.05 mm to 0.3 mm.

[0037] W powder with an average particle size of 15 μm and Re powder with an average particle size of 5 μm were mixed in a slurry form using an alcohol-based solution so that the Re content (%) was the content (%) of Examples 1 to 8 listed in Table 1. The resulting mixed powder was press-molded to obtain a green body. Next, the green body was pre-sintered in a hydrogen atmosphere at 1300°C, and then sintered in a hydrogen atmosphere at 3000°C to obtain a sintered body. The sintered body was subjected to a first rolling process at 1500°C with a cross-sectional area reduction rate of 10%. After the first rolling process, heat treatment was performed by electrical heating to perform a non-uniform treatment. Sintered bodies were also produced using mixed powders with Re contents of 10% and 31%, designated as Examples 9 and 10.

[0038] Next, rolling was performed at 1500°C with a surface reduction rate of 50%, followed by a second rolling process at 1300°C with a surface reduction rate of 10%. The ReW rod material after the second rolling process was recrystallized in a hydrogen atmosphere at 2000°C. The recrystallized ReW rod material was then subjected to a third rolling process at 1300°C with a surface reduction rate of 25% and drawn to a diameter of 2 mm. Further drawing was performed to produce a φ0.3 mm ReW wire. During this drawing process, annealing heat treatment was performed in an oxidizing atmosphere at the temperatures listed in Table 1 when the diameters reached φ1 mm and φ0.4 mm, resulting in the ReW wires of Examples 1 to 8. Furthermore, the drawing process was performed at a processing temperature of 600°C in Examples 4 to 8 and 900°C in Examples 1 to 3. More specifically, in Examples 4 to 8, the temperature for wiredrawing from 2 mm to 1 mm in diameter was 600° C., annealing heat treatment was performed when the diameter was 1 mm, the temperature for wiredrawing from 1 mm to 0.4 mm in diameter was 600° C., annealing heat treatment was performed when the diameter was 0.4 mm, and the temperature for wiredrawing from 0.4 mm to 0.3 mm in diameter was 600° C. Examples 1 to 3 were similar, except that the processing temperature was 900° C.

[0039] Using the above-mentioned processing method and processing conditions, the products shown in Table 1 were manufactured. The manufactured ReW wires had a mixture layer on the surface. Regarding the Re content, Example 9, which contained 10%, did not achieve the target tensile strength, and Example 10, which contained 31%, could not be processed in the upstream process and could not be tested. Table 1 shows the Re content (wt %), the annealing temperature (°C) at a diameter of 1 mm, the annealing temperature (°C) at a diameter of 0.4 mm, the percentage (%) of the area ratio occupied by crystal orientations within 15° of the <101> parallel to the ND (wiredrawing) direction in the central portion, the percentage (%) of the area ratio occupied by crystal orientations within 5° of the <101> parallel to the ND (wiredrawing) direction in the central portion, the percentage (%) of the area ratio occupied by crystal orientations within 15° of the <101> parallel to the ND (wiredrawing) direction in the peripheral portion, the percentage (%) of the area ratio occupied by crystal orientations within 15° of the <227> parallel to the ND (wiredrawing) direction in the peripheral portion, the average grain size (µm) on the crystal grain map of the central portion, the maximum grain size (µm) on the crystal grain map of the central portion, and the ratio of the average grain size at the central portion to the average grain size in the peripheral portion (central portion / peripheral portion). In the ReW wires of Examples 2 to 8, the area ratio (%) of crystal orientations within 15° of the <101> parallel to the ND (wiredrawing) direction in the center portion satisfies 90% to 99.9%.

[0040]

[0041] Measurement samples were taken from the ReW wire of each example, where both ends had been removed as described above. EBSD analysis was performed using the method described above to determine the area ratio of the crystal orientation and the crystal grain size. After the samples were taken, 5 kg of wire was used as a wire and drawn to a diameter of 0.20 mm. The number of breaks of the ReW wire until it was completed to a diameter of 0.20 mm was evaluated. The number of breaks is the total number of breaks that occurred during the wiredrawing process to finish a total of 5 kg of wire to a diameter of 0.20 mm. For example, if the wire breaks and splits into two pieces, the number of breaks is recorded as 1. If the wire breaks and splits into five pieces, the number of breaks is recorded as 4. As can be seen from Table 1, the ReW wire according to the embodiment can suppress breakage and can meet the demand for longer lengths when used in medical suture needles.

[0042] Although several embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be embodied in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included within the scope and spirit of the invention, as well as within the scope of the invention and its equivalents as set forth in the claims. Furthermore, the above-described embodiments can be implemented in combination with each other.

[0043] The following are embodiments of the invention. <1> A tungsten wire made of a tungsten alloy containing rhenium, wherein, when EBSD analysis is performed on a unit area of ​​40 μm × 40 μm at a center portion located within 100 μm of the central axis in a wire radial cross section perpendicular to the wiredrawing direction of a main body portion of the tungsten wire, the proportion of the area ratio of crystal orientations within a 15° misorientation from the <101> parallel to the wiredrawing direction on the IPF map is 90% to 99.9% within the measurement field of view. <2> The tungsten wire according to <1>, wherein, on the IPF map, the proportion of the area ratio of crystal orientations within a 5° misorientation from the <101> parallel to the wiredrawing direction on the IPF map is 88% to 98% within the measurement field of view. <3> The tungsten wire according to any one of <1> to <2>, wherein, when EBSD analysis is performed on a unit area of ​​40 μm × 40 μm in an outer peripheral portion of the main body of the tungsten wire, the proportion of an area ratio of crystal orientations within a 15° misorientation from a <101> crystal orientation parallel to the wiredrawing direction on an IPF map is 70% to 93% within the measurement field of view. <4> The tungsten wire according to any one of <1> to <3>, wherein, on an IPF map of the outer peripheral portion of the main body of the tungsten wire, the proportion of an area ratio of crystal orientations within a 15° misorientation from a <227> crystal orientation parallel to the wiredrawing direction on an IPF map is 3% to 20% within the measurement field of view. <5> The tungsten wire according to any one of <1> to <4>, wherein, on a crystal grain map of the central portion of the main body of the tungsten wire, the average grain size is 0.15 μm to 0.23 μm. <6> The tungsten wire according to any one of <1> to <5>, wherein, on a grain map of the central portion of the main body portion of the tungsten wire, the maximum grain size is 0.8 μm or more and 2.0 μm or less. <7> The tungsten wire according to any one of <1> to <6>, <7> On grain maps of the central portion of the main body portion of the tungsten wire and the peripheral portion of the main body portion of the tungsten wire, the ratio of average grain sizes in the central portion to the peripheral portion is greater than 1.00 and less than 1.20.<8> The tungsten wire according to any one of <1> to <7>, wherein the tungsten alloy has a rhenium content of 11 wt% or more and 30 wt% or less. <9> The tungsten wire according to any one of <1> to <8>, wherein the diameter of the tungsten wire is 0.05 mm or more and 0.3 mm or less.

[0044] S 0 ...cross section (measurement surface) perpendicular to the axial direction of the embodiment, ND...cross section normal (axial) direction (Normal Direction), TD...cross section horizontal (radial) direction (Transverse Direction), RD...cross section horizontal direction perpendicular to TD (Reference Direction), 1...periphery, 2...center.

Claims

1. A tungsten wire made of a tungsten alloy containing rhenium, wherein, when EBSD analysis is performed on a unit area of ​​40 μm x 40 μm at a center portion located within 100 μm concentrically from the central axis in a wire radial cross section perpendicular to the wiredrawing direction in a main body portion of the tungsten wire, the area ratio of crystal orientations within an orientation difference of 15° from <101> parallel to the wiredrawing direction on an IPF map is 90% or more and 99.9% or less within the measurement field of view.

2. The tungsten wire according to claim 1, wherein on the IPF map, the area ratio of crystal orientations within a 5° misorientation from the <101> parallel to the wiredrawing direction is 88% or more and 98% or less within the measurement field of view.

3. The tungsten wire according to any one of claims 1 and 2, wherein, when EBSD analysis is performed on a unit area of ​​40 μm × 40 μm in an outer peripheral portion located within 50 μm inward from the outer periphery of a main body of the tungsten wire, the area ratio of crystal orientations within an orientation difference of 15° from <101> parallel to the wiredrawing direction on the IPF map is 70% or more and 93% or less within the measurement field of view.

4. The tungsten wire according to claim 3, wherein on the IPF map of the outer periphery of the main body of the tungsten wire, the area ratio of crystal orientations within an orientation difference of 15° from <227> parallel to the wiredrawing direction is 3% or more and 20% or less within the measurement field of view.

5. The tungsten wire according to claim 1, wherein an average grain size on a grain map of the central portion of the main body of the tungsten wire is 0.15 μm or more and 0.23 μm or less.

6. The tungsten wire according to claim 1, wherein the maximum grain size on a crystal grain map of the central portion of the main body of the tungsten wire is 0.8 μm or more and 2.0 μm or less.

7. The tungsten wire according to claim 3, wherein on a grain map of the central portion of the tungsten wire body and the peripheral portion of the tungsten wire body, the ratio of average grain size of the central portion to that of the peripheral portion is greater than 1.00 and less than 1.

20.

8. The tungsten wire according to any one of claims 1 to 2, wherein the tungsten alloy has a rhenium content of 11 wt% or more and 30 wt% or less.

9. The tungsten wire according to any one of claims 1 to 2, wherein the diameter of the tungsten wire is 0.05 mm or more and 0.3 mm or less.

Citation Information

Patent Citations

  • Rhenium-tungsten alloy material excellent in workability and its manufacture

    JP1991219039A

  • Process for producing tungsten wire

    WO2009066659A1

  • Metallic material composed of tungsten or molybdenum, production of the metallic material and secondary product material using the metallic material

    JP1999092851A

  • Steel wire rod and method of producing steel wire rod

    JP2016056438A

  • Cathode component for discharge lamp, and discharge lamp

    WO2020105644A1