Particulate water absorbent, absorber containing said particulate water absorbent, and sanitary product containing said absorber

A surface-crosslinked polyacrylic acid (salt)-based resin particulate water-absorbing agent addresses the issue of liquid return in sanitary products by meeting specific retention capacity parameters, ensuring effective liquid retention under varying pressures and rapid absorption, thereby improving product performance.

WO2024204126A1PCT designated stage expired Publication Date: 2024-10-03NIPPON SHOKUBAI CO LTD

Patent Information

Application Number
PCT/JP2024/011819
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing particulate water-absorbing agents in sanitary products, such as diapers, face challenges in reducing liquid return during actual use, as the standard measurement parameters do not accurately represent the conditions encountered during use, where pressure varies and liquid absorption occurs over shorter periods.

Method used

A particulate water-absorbing agent with a surface-crosslinked polyacrylic acid (salt)-based resin that meets specific parameters, including Short-time Retention Capacity under No Pressure (SRC(NP)) > 50.0 g/g and SRC (4.83 kPa) > 41.5 g/g, ensuring effective liquid retention under varying pressures and rapid absorption.

Benefits of technology

The agent significantly reduces liquid return in sanitary products by maintaining excellent liquid retention capacity both under no pressure and high pressure conditions, enhancing the performance of sanitary products during actual use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

Provided is a particulate water absorbent which can be used for manufacturing a sanitary product capable of further reducing absorbed liquid rewetting during actual use. The particulate water absorbent demonstrates a water absorption magnification of more than 50 g / g when a swollen gel, which is obtained by bringing the particulate water absorbent into contact with 0.9% sodium chloride aqueous solution for 10 minutes, is left to stand under no pressure for one minute, and demonstrates a water absorption magnification of more than 41.5 g / g when the swollen gel is left to stand under a pressure of 4.83 kPa for one minute.
Need to check novelty before this filing date? Find Prior Art

Description

Particulate water-absorbing agent, absorbent body containing said particulate water-absorbing agent, and sanitary product containing said absorbent body

[0001] The present invention relates to a particulate water-absorbing agent, an absorbent body containing the particulate water-absorbing agent, and a sanitary product containing the water-absorbing body.

[0002] A water-absorbent resin (SAP / Super Absorbent Polymer) is a water-swellable, water-insoluble polymer gelling agent. Particulate water-absorbing agents containing water-absorbent resins as their main component are used in absorbent articles for a variety of applications, including hygiene products such as disposable diapers, sanitary napkins, and adult incontinence products, soil water-retaining agents for agricultural and horticultural use, and industrial water-stopping agents. Many monomers and hydrophilic polymers have been proposed as raw materials for such water-absorbent resins. From the viewpoints of performance and cost, polyacrylic acid (salt)-based water-absorbent resins using acrylic acid and / or its salt as a monomer are most commonly used as the water-absorbent resin.

[0003] With the advancement of performance in disposable diapers, which are the main application of particulate water-absorbing agents, many functions (physical properties) are required of the particulate water-absorbing agent. One of the many functions is the ability to have excellent liquid-retaining power and reduce liquid return even when pressure is applied from the outside while the particulate water-absorbing agent is in a swollen state.

[0004] Absorbent articles, such as sanitary products like disposable diapers, are not replaced every time a liquid to be absorbed, such as urine, is discharged, but are usually subjected to multiple discharges of liquid into the absorbent article. The particulate water-absorbing agent that has absorbed the liquid becomes swollen. Therefore, a user may use an absorbent article having a particulate water-absorbing agent in a swollen state. When in this swollen state, the particulate water-absorbing agent is required to have excellent liquid retention and a function of reducing liquid return, regardless of the wearer's daily activities, especially in situations where pressure is applied to the particulate water-absorbing agent from the outside, such as when the wearer's weight is applied to the absorbent article. Note that the state where the wearer's weight is applied to the absorbent article includes, for example, when the wearer is lying on his / her back or sitting.

[0005] An example of a particulate water-absorbing agent having the above-mentioned function is the particulate water-absorbing agent described in Patent Document 1. Patent Document 1 proposes a particulate water-absorbing agent in which the water absorption capacity under pressure (AAP) (2.06 kPa) at a pressure condition of 2.06 kPa, the water absorption capacity without pressure (CRC), and the water absorption capacity under pressure after swelling (RCAP) (2.06 kPa) have a specific relationship. Here, RCAP (2.06 kPa) represents the weight change of the particulate water-absorbing agent before and after an operation in which the particulate water-absorbing agent is immersed in a 0.9 wt % sodium chloride aqueous solution for 1 hour to form a swollen gel, and then left to stand under a load of 2.06 kPa for 1 minute, i.e., the water absorption capacity.

[0006] International Publication No. 2021 / 201177 Pamphlet

[0007] However, particularly when a sanitary product such as an adult diaper is actually used, the particulate water absorbing agent contained in the sanitary product needs to absorb a large amount of liquid such as urine under no pressure in a time shorter than the immersion time (1 hour) in the measurement of the RCAP (2.06 kPa). Furthermore, when the sanitary product is actually used, it is considered that the particulate water absorbing agent in a swollen state is maintained under no pressure or a pressure higher than 2.06 kPa is applied to the swollen particulate water absorbing agent in accordance with the user's movements.

[0008] Therefore, it cannot be said that the RCAP (2.06 kPa) is a parameter corresponding to the conditions when the sanitary product is actually used. Therefore, the sanitary product including the particulate water-absorbing agent described in Patent Document 1 has room for improvement in terms of reducing the return of absorbed liquid when actually used.

[0009] The object of the present invention has been made in consideration of the above-mentioned problems, and its object is to provide a particulate water-absorbing agent that can be used to manufacture sanitary products that can further reduce the return of absorbed liquid during actual use.

[0010] The present inventors have found two kinds of new parameters corresponding to the conditions of actual use of the sanitary product, and have found that a particulate water-absorbing agent having the parameters within a specific range can solve the above problems, thereby arriving at the present invention. The parameters are a parameter corresponding to the water absorption capacity when a swollen gel obtained by swelling the particulate water-absorbing agent in a short time is held under no pressure, and a parameter corresponding to the water absorption capacity when the swollen gel is held under high pressure.

[0011] That is, one aspect of the present invention relates to a particulate water-absorbing agent containing a surface-crosslinked polyacrylic acid (salt)-based water-absorbing resin as a main component, which satisfies the following formula (A) and formula (B): SRC(NP)>50.0 g / g (A) SRC(4.83 kPa)>41.5 g / g (B) Here, the SRC(NP) is measured by a method including the following steps (a) to (c).

[0012] (a) The particulate water-absorbing agent (W 0 ) [g] is brought into contact with a 0.9% aqueous sodium chloride solution (hereinafter referred to as the "test liquid") for 10 minutes without applying a load, to obtain a swollen gel.

[0013] (b) separating the swollen gel obtained in step (a) from the test liquid;

[0014] (c) The weight (W) of the swollen gel separated in step (b) 1 ) [g], and calculate the SRC (NP) of the particulate water-absorbing agent based on the following formula (1); SRC (NP) [g / g] = W 1 / W 0 (1) The SRC (4.83 kPa) is measured by carrying out a method including steps (c') to (e') described below in place of step (c) in the method including steps (a) to (c).

[0015] (c') A load of 4.83 kPa is applied to the swollen gel separated in step (b) for 1 minute.

[0016] (d') The exudate exuded from the swollen gel in step (c') is removed.

[0017] (e') The weight (W 2 ) [g] is measured, and the SRC (4.83 kPa) is calculated based on the following formula (2); SRC (4.83 kPa) [g / g] = W 2 / W 0 (2)

[0018] The particulate water-absorbing agent according to one embodiment of the present invention has an effect that it can be used to manufacture sanitary products that can further reduce the return of absorbed liquid during actual use.

[0019] The present invention will now be described with reference to the best mode. Throughout this specification, singular expressions should be understood to include the plural concept unless otherwise specified. Therefore, singular articles (e.g., "a," "an," "the," etc. in English) should be understood to include the plural concept unless otherwise specified. Furthermore, terms used in this specification should be understood to have the meaning commonly used in the art unless otherwise specified. Therefore, unless otherwise defined, all technical and scientific terms used in this specification have the same meaning as commonly understood by those skilled in the art to which this invention belongs. In the event of any conflict, the present specification (including definitions) will take precedence. The present invention is not limited to the following embodiments, and various modifications can be made within the scope of the claims.

[0020] [1] Definition of Terms (1-1) "Water-absorbent resin" In the present invention, the "water-absorbent resin" refers to a crosslinked polymer that has "swellability" and "insolubility" and that absorbs a liquid, swells, and becomes an insoluble gel, and satisfies the following physical properties. That is, the "water-swellable" crosslinked polymer satisfies the physical properties of a CRC of 5 g / g or more as defined in ERT441.2-02, and an Ext of 50 wt% or less as defined in ERT470.2-02.

[0021] The water-absorbing resin can be appropriately designed depending on its application, and is not particularly limited, but is preferably a hydrophilic cross-linked polymer obtained by cross-linking an unsaturated monomer having a carboxyl group. In addition, the water-absorbing resin is not limited to a form in which the total amount (100% by weight) is a polymer, and may be a water-absorbing resin composition containing additives and the like within a range that satisfies the above physical properties (CRC, Ext).

[0022] Furthermore, the water-absorbent resin in one embodiment of the present invention is not limited to a final product, but may also refer to an intermediate in the manufacturing process of the water-absorbent resin (for example, a hydrogel-like crosslinked polymer after polymerization, a dried polymer after drying, and a water-absorbent resin powder before surface crosslinking, etc.). In this specification, all of these are collectively referred to as a "water-absorbent resin". Note that, although the shape of the water-absorbent resin may be a sheet, fiber, film, particle, gel, etc., the water-absorbent resin in one embodiment of the present invention is mainly in the particle shape (powder).

[0023] (1-2) "Particulate Water Absorbing Agent" In this specification, the water absorbing agent contains a water absorbent resin as a main component. In this specification, the particulate water absorbing agent means a particulate (also known as powder) water absorbing agent (containing water absorbent resin particles as a main component), and is referred to as a particulate water absorbing agent whether it is a single particle of particulate water absorbing agent or a plurality of particles of particulate water absorbing agent. "Particulate" means having the form of particles, and a particle refers to a small granular solid or liquid object having a measurable size (JIS Industrial Terminology Dictionary, 4th Edition, p. 2002). In this specification, the particulate water absorbing agent may also be simply referred to as a water absorbing agent.

[0024] In this specification, the aqueous liquid is not limited to water, but may also be urine, blood, sweat, feces, waste liquid, moisture, steam, ice, a mixture of water with an organic solvent and / or an inorganic solvent, rainwater, groundwater, etc. As long as it contains water, it is not particularly limited. Preferred examples of the aqueous liquid include urine, menstrual blood, sweat, and other body fluids.

[0025] A particulate water-absorbing agent according to one embodiment of the present invention is suitable for use as a sanitary material for absorbing aqueous liquids. The particulate water-absorbing agent is primarily composed of a surface-crosslinked polyacrylic acid (salt)-based water-absorbing resin (particles) (hereinafter simply referred to as a polyacrylic acid (salt)-based water-absorbing resin). In other words, the surface-crosslinked polyacrylic acid (salt)-based water-absorbing resin is preferably contained in the particulate water-absorbing agent in an amount of 60 to 100% by weight, 70 to 100% by weight, 80 to 100% by weight, or 90 to 100% by weight. The particulate water-absorbing agent may optionally contain one or more materials selected from the group consisting of other water-absorbent resin particles, water, and additives. The additives may include inorganic colloid particles, water-insoluble inorganic particles, water-soluble polyvalent metal cation-containing compounds, and the like. The particulate water-absorbing agent preferably has a water content of 0.2 to 30% by weight. In other words, a water-absorbent resin composition formed by combining these components also falls within the scope of the particulate water-absorbing agent.

[0026] The upper limit of the content of the polyacrylic acid (salt)-based water-absorbing resin in the water-absorbing agent is 99% by weight, particularly about 95% by weight, 90% by weight, or 85% by weight, and preferably the water-absorbing agent further contains water and / or an additive (inorganic colloid particles, water-insoluble inorganic particles, water-soluble polyvalent metal cation-containing compound) described below.

[0027] Furthermore, the particulate water-absorbing agent according to one embodiment of the present invention may contain a polyacrylic acid (salt)-based water-absorbing resin as a main component, and may also contain other water-absorbing resins. Examples of the other water-absorbing resins include polysulfonic acid (salt)-based water-absorbing resins, maleic anhydride (salt)-based water-absorbing resins, polyacrylamide-based water-absorbing resins, polyvinyl alcohol-based water-absorbing resins, polyethylene oxide-based water-absorbing resins, polyaspartic acid (salt)-based water-absorbing resins, polyglutamic acid (salt)-based water-absorbing resins, polyalginic acid (salt)-based water-absorbing resins, starch-based water-absorbing resins, and cellulose-based resins. The number of types of the other water-absorbing resins may be one or more.

[0028] (1-3) "Polyacrylic acid (salt)" and "Polyacrylic acid (salt)-based water-absorbent resin" In one embodiment of the present invention, "polyacrylic acid (salt)" refers to polyacrylic acid and / or its salt. Furthermore, a "polyacrylic acid (salt)-based water-absorbent resin" is a polyacrylic acid (salt) cross-linked polymer that contains, as a main component, structural units derived from acrylic acid and / or its salt (hereinafter referred to as "acrylic acid (salt)") as repeating units and has an internal cross-linked structure. The polyacrylic acid (salt)-based water-absorbent resin is preferably surface-cross-linked.

[0029] The polyacrylic acid (salt)-based water-absorbing resin is preferably in a particulate form (also called powder form) among the particulate water-absorbing agents.

[0030] The term "main component" means that the amount (content) of acrylic acid (salt) used is usually 50 to 100 mol %, preferably 70 to 100 mol %, more preferably 90 to 100 mol %, and even more preferably substantially 100 mol %, based on the total amount of monomers (excluding the internal crosslinking agent) used in the polymerization.

[0031] (1-4) "EDANA" and "ERT" "EDANA" is an abbreviation for European Disposables and Nonwovens Associations, and "ERT" is an abbreviation for EDANA Recommended Test Methods, a European standard (almost a global standard) for measuring the properties of water-absorbent resins. In the present invention, unless otherwise specified, the physical properties of the water-absorbent resin are measured in accordance with the original ERT (revised in 2002 / publicly known document).

[0032] (1-4-1) “CRC” (ERT441.2-02) “CRC” is an abbreviation for Centrifuge Retention Capacity, and means the water absorption capacity under no load of a particulate water-absorbing agent or a water-absorbing resin (sometimes referred to as “water absorption capacity”).

[0033] Specifically, the absorbency (unit: g / g) refers to a value obtained by placing 0.2 g of a particulate water-absorbing agent or a water-absorbing resin in a nonwoven fabric bag, immersing the bag in a large excess of a 0.9 wt % aqueous solution of sodium chloride for 30 minutes to allow the bag to freely swell, and then draining the water using a centrifuge (250 G).

[0034] (1-4-2) "PSD" (ERT420.2-02) "PSD" is an abbreviation for Particle Size Distribution, and means the particle size distribution of a particulate water-absorbing agent or a water-absorbing resin measured by sieve classification.

[0035] The weight-average particle diameter (D50) and the logarithmic standard deviation (σζ) of particle size distribution are measured in the same manner as in "(3) Mass-Average Particle Diameter (D50) and Logarithmic Standard Deviation (σζ) of Particle Diameter Distribution" described in U.S. Pat. No. 7,638,570.

[0036] (1-5) Others In this specification, the range "X to Y" means "X or more and Y or less." Unless otherwise noted, the unit of weight "t (ton)" means "Metric ton," and "ppm" means "weight ppm" or "mass ppm." Furthermore, "weight" and "mass," "parts by weight" and "parts by mass," "wt %" and "mass %" are treated as synonyms. Furthermore, "~ acid (salt)" means "~ acid and / or its salt," and "(meth)acrylic" means "acrylic and / or methacrylic."

[0037] For convenience, "liter" may be abbreviated as "l" or "L" and "weight %" as "wt%." Furthermore, when measuring trace components, amounts below the detection limit are expressed as N.D. (Non Detected).

[0038] [2] Particulate Water Absorbing Agent A particulate water absorbing agent according to one embodiment of the present invention (hereinafter referred to as "the particulate water absorbing agent of the present invention") is a particulate water absorbing agent containing a surface-crosslinked polyacrylic acid (salt)-based water-absorbing resin as a main component, and satisfies the following formula (A) and formula (B): SRC(NP)>50.0 g / g (A) SRC(4.83 kPa)>41.5 g / g (B) Here, the SRC(NP) is measured by a method including the following steps (a) to (c):

[0039] (a) The particulate water-absorbing agent (W 0 ) [g] is brought into contact with a 0.9% aqueous sodium chloride solution (hereinafter referred to as the "test liquid") for 10 minutes without applying a load, to obtain a swollen gel.

[0040] (b) separating the swollen gel obtained in step (a) from the test liquid;

[0041] (c) The weight (W) of the swollen gel separated in step (b) 1 ) [g], and calculate the SRC (NP) of the particulate water-absorbing agent based on the following formula (1); SRC (NP) [g / g] = W 1 / W 0 (1) The SRC (4.83 kPa) is measured by carrying out a method including steps (c') to (e') described below in place of step (c) in the method including steps (a) to (c).

[0042] (c') A load of 4.83 kPa is applied to the swollen gel separated in step (b) for 1 minute.

[0043] (d') The exudate exuded from the swollen gel in step (c') is removed.

[0044] (e') The weight (W 2 ) [g] is measured, and the SRC (4.83 kPa) is calculated based on the following formula (2); SRC (4.83 kPa) [g / g] = W 2 / W 0(2) The SRC(NP) is a parameter representing the amount of liquid retained in the particulate water-absorbing agent when the particulate water-absorbing agent is allowed to absorb a liquid in a short time, causing it to swell, and then held under no pressure. Note that "SRC(NP)" is an abbreviation for Short-time Retention Capacity (No Pressure). The SRC(4.83 kPa) is a parameter representing the amount of liquid retained in the particulate water-absorbing agent when the particulate water-absorbing agent is allowed to absorb a liquid in a short time, causing it to swell, and then held under high pressure.

[0045] The particulate water-absorbing agent of the present invention satisfies the above formula (A) and formula (B). Therefore, the particulate water-absorbing agent of the present invention can absorb a large amount of liquid in a short time, and is excellent in the amount of liquid that can be retained both when the particulate water-absorbing agent is retained in a swollen state without pressure and when the particulate water-absorbing agent is retained under high pressure. Here, the ability to absorb a large amount of liquid in a short time and the ability to retain a large amount of liquid when the particulate water-absorbing agent is retained in a swollen state without pressure and when the particulate water-absorbing agent is retained under high pressure are properties necessary for further reducing the liquid return during actual use of the sanitary product. This point is as described in the above section "Problem to be Solved by the Invention." Therefore, the particulate water-absorbing agent of the present invention can be used to manufacture sanitary products that can further reduce the return of absorbed liquid during actual use.

[0046] In the step (a), the particulate water-absorbing agent W 0[g] is brought into contact with a 0.9% sodium chloride aqueous solution (hereinafter referred to as "test liquid") adjusted to 23±1°C for 10 minutes without applying a load. Here, the water absorption capacity of a particulate water-absorbing agent is generally limited when a load is applied. Therefore, the above-mentioned "contact for 10 minutes without applying a load" means that the particulate water-absorbing agent is brought into contact with a large excess of test liquid without limiting its water absorption capacity by a load, and the particulate water-absorbing agent is maintained in a state where it can sufficiently absorb the test liquid for 10 minutes, thereby allowing it to freely swell. The above-mentioned "contact" means that the particulate water-absorbing agent is brought into contact with the test liquid and brought into a state where it can absorb the test liquid. Here, the particulate water-absorbing agent and the test liquid may be brought into contact with each other via a liquid-permeable member such as a nonwoven fabric or a wire mesh. Therefore, in the step (a), the amount of test liquid used and the conditions such as the shape and size of the measuring device are appropriately adjusted so that the test liquid used is not insufficient and the free swelling of the particulate water-absorbing agent is not hindered during the 10 minutes.

[0047] The container for carrying out the step (a) is not particularly limited, and may be, for example, a cylinder equipped with a piston. The bottom of the cylinder is preferably fitted with a wire mesh that is impermeable to the particulate water-absorbing agent and swollen gel described below and allows the test liquid and exudate described below to flow in or to be discharged. For example, the cylinder and piston used in the Gel Bed Permeability Test described in U.S. Patent Publication No. 8,269,060 may be used as the container.

[0048] The specific method for carrying out the step (a) is not particularly limited. For example, when a cylinder equipped with a piston is used, the method may include the following steps (a1) to (a3):

[0049] (a1) First, measure the total weight of the cylinder and the piston, and set the value as W a [g].

[0050] (a2) Following the step (a1), a step of measuring approximately 0.9 g of a sample of the particulate water-absorbing agent to be measured and uniformly scattering it on the bottom surface of the cylinder. Here, the sample is accurately weighed in advance, and W 0 Let [g].

[0051] (a3) subsequent to step (a2), the cylinder is placed in a large excess of 0.9% aqueous sodium chloride solution as a test liquid, and the uniformly dispersed sample is brought into contact with the test liquid for 10 minutes to obtain a swollen gel. In step (a3), the sample absorbs the test liquid and swells without being subjected to a load, thereby obtaining a swollen gel.

[0052] The shape and size of the measuring device are not limited. From the viewpoint of improving the accuracy of the measurement of the SRC (NP) and the SRC (4.83 kPa), the device used for the measurement should have a bottom area of ​​19 to 40 cm 2 The particulate water-absorbing agent used in the measurement has a basis weight of 250 to 350 g / m 2 As an example, when the measurement is carried out using a cylinder and a piston used in a Gel Bed Permeability test described in U.S. Patent Publication No. 8,269,060 as the measurement device, the amount of the particulate water-absorbing agent used is preferably 0.9 g.

[0053] In the step (b), the swollen gel obtained in the step (a) is separated from the test liquid. This step means terminating the contact between the particulate water-absorbing agent and the test liquid in the step (a) and removing the test liquid (hereinafter also referred to as "excess water") that is present between the hydrogel particles of the swollen gel obtained in the step (a) and that is not absorbed by the hydrogel particles. The method for removing the excess water is not particularly limited. For example, the method may include lifting the swollen gel obtained in the step (a) from the large excess of test liquid, placing it on a sieve, and allowing it to stand to drain. The draining time is preferably about 1 minute. The draining is continued until the excess liquid is removed from the hydrogel particles. The "excess water removed" state refers to a state in which no water droplets fall from the measuring device for 5 seconds.

[0054] When removing excess water, the surrounding environment is preferably room temperature (20 to 25°C) and normal pressure (1 atmosphere) to match the environment in which sanitary products such as diapers are used.

[0055] In the step (b), in order to make the thickness of the swollen gel uniform, it is preferable to lift the swollen gel from the test liquid with a piston or the like placed on the swollen gel. Furthermore, it is preferable to drain the liquid from the swollen gel while the piston or the like remains on the swollen gel. The load applied by the piston is preferably 0.22 to 0.28 kPa, more preferably 0.24 to 0.26 kPa, and particularly preferably 0.25 kPa, from the viewpoint of making the thickness of the swollen gel uniform without applying an excessive load to the swollen gel.

[0056] In the step (c), the weight of the swollen gel separated in the step (b), i.e., the swollen gel separated from the test liquid, is measured. The method for measuring the weight of the swollen gel is not particularly limited, and the weight can be measured using a commercially available weighing scale. The steps (a) to (c) can be performed in a state where the particulate water-absorbing agent and the swollen gel are placed in a container composed of a cylinder, a piston, or the like. In this case, the weight of the container is measured in advance, and the total weight of the container and the swollen gel is measured. The weight of the swollen gel can be calculated by subtracting the weight of the container from the total weight. If the test liquid adheres to the container as water droplets, the water droplets are removed using, for example, Kimwipes or the like before measuring the weight.

[0057] In the step (c), the weight W of the particulate water-absorbing agent before swelling obtained in the step (a) is 0 [g] and the weight W of the swollen gel obtained in step (c). 1 The SRC(NP) value is calculated using the SRC(NP) [g / g] and the SRC(NP) [g / g] according to the following formula (1): 1 / W 0 (1) In step (c'), a load of 4.83 kPa is applied to the swollen gel separated in step (b), i.e., the swollen gel separated from the test liquid, for one minute. As in step (b), the ambient environment during application of the load to the swollen gel is preferably room temperature (20-25°C) and normal pressure (1 atmosphere) to match the usage environment of sanitary products such as diapers. The load can be applied, for example, by placing a piston on the swollen gel evenly distributed on the bottom surface of a cylinder and then placing a weight on the piston capable of applying a load of 4.83 kPa to the swollen gel. Application of the load causes a portion of the liquid absorbed by the swollen gel in step (b) to exude from the swollen gel. Hereinafter, this exuded liquid will be referred to as "exudate."

[0058] In the step (d'), the exudate exuded from the swollen gel obtained in the step (c') is removed. That is, the exudate exuded from the swollen gel after a load of 4.83 kPa is applied for 1 minute is removed. The method for removing the exudate is not particularly limited, and examples thereof include a method of performing the following steps (i) and (ii):

[0059] (i) A piston is placed on the swollen gel evenly spread on a wire mesh provided on the bottom of the cylinder, and with a load of 4.83 kPa placed on the piston, the piston is placed on a sieve to drain the liquid.

[0060] (ii) removing the exudate that has exuded onto the piston using a dropper;

[0061] In the step (e'), the weight of the swollen gel obtained in the step (d'), i.e., the swollen gel after the exudate has been removed, is measured. The method for measuring the weight of the swollen gel is not particularly limited, and the weight can be measured using a commercially available weighing scale. The steps (a), (b), and (c') to (e') can be performed in a state in which the particulate water-absorbing agent and the swollen gel are placed in a container composed of a cylinder, a piston, a weight, and the like. In this case, the weight of the container is measured in advance, and the total weight of the container and the swollen gel is measured. The weight of the swollen gel can be calculated by subtracting the weight of the container from the total weight. If the test liquid and the exudate adhere to the container as water droplets, the water droplets remaining in the container are removed using, for example, Kimwipes before measuring the weight.

[0062] In the step (e'), the weight W of the particulate water-absorbing agent before swelling obtained in the step (a) is 0 [g] and the weight W of the swollen gel obtained in the step (e'). 2 The SRC (4.83 kPa) value is calculated using the SRC (4.83 kPa) [g / g] and the SRC (4.83 kPa) [g / g] = W 2 / W 0(2) Furthermore, the "liquid return" that is usually used to evaluate the physical properties of a water-absorbent resin is an evaluation of an absorbent sheet (absorbent body) in which an absorbent layer containing a water-absorbent resin (water-absorbing agent) and pulp or the like is laminated with a nonwoven fabric or the like, and is not an evaluation of the water-absorbent resin (water-absorbing agent) itself. Note that the "liquid return" is sometimes referred to as the amount of return or Re-Wet.

[0063] (2-1) SRC(NP) The method for measuring the SRC(NP) is not particularly limited as long as it includes the above-described steps (a) to (e). The SRC(NP) can be measured, for example, by the method described in the Examples of the present application.

[0064] The lower limit of the SRC(NP) is a value exceeding 50.0 g / g, preferably a value exceeding 54.0 g / g, more preferably a value exceeding 56.0 g / g, even more preferably a value exceeding 58.0 g / g, and particularly preferably 59.0 g / g or more. The upper limit of the SRC(NP) is not particularly limited and is usually 70.0 g / g or less. Since the particulate water-absorbing agent of the present invention has an SRC(NP) exceeding the preferred lower limit, it can absorb a large amount of liquid in a short time, and can sufficiently retain the large amount of liquid when held in a swollen state without pressure. As a result, the sanitary product containing the particulate water-absorbing agent of the present invention can further reduce the return of absorbed liquid during actual use.

[0065] (2-2) SRC (4.83 kPa) The method for measuring the SRC (4.83 kPa) is not particularly limited as long as it includes the above-mentioned steps (a), (b), and (c') to (e'). The SRC (4.83 kPa) can be measured, for example, by the method described in the Examples of the present application.

[0066] The lower limit of the SRC (4.83 kPa) is a value exceeding 41.5 g / g, preferably a value exceeding 42.0 g / g, more preferably a value exceeding 42.5 g / g, and particularly preferably 43.0 g / g. The upper limit of the SRC (4.83 kPa) is not particularly limited and is usually 50.0 g / g or less. Since the particulate water-absorbing agent of the present invention has an SRC (4.83 kPa) exceeding the preferred lower limit, the particulate water-absorbing agent can absorb a larger amount of liquid in a short time, and can sufficiently retain the large amount of liquid when held under a high pressure of 4.83 kPa in a swollen state. As a result, the sanitary product containing the particulate water-absorbing agent of the present invention can further reduce the return of absorbed liquid during actual use.

[0067] (2-3) CRC (Centrifuge Retention Capacity) (ERT441.2-02) “CRC” is an abbreviation for Centrifuge Retention Capacity, and means the water absorption capacity under no load of a particulate water-absorbing agent or a water-absorbent resin (sometimes referred to as “water absorption capacity”).

[0068] Specifically, the absorbency (unit: g / g) refers to a value obtained by placing 0.2 g of a particulate water-absorbing agent or a water-absorbing resin in a nonwoven fabric bag, immersing the bag in a large excess of a 0.9 wt % aqueous solution of sodium chloride for 30 minutes to allow the bag to freely swell, and then draining the water using a centrifuge (250 G).

[0069] The lower limit of the CRC (centrifuge retention capacity) of the particulate water-absorbing agent of the present invention is preferably 35 g / g or more, more preferably 36 g / g or more, even more preferably 38 g / g or more, even more preferably 39 g / g or more, particularly preferably 40 g / g or more, and even particularly preferably 41 g / g or more. When the CRC is 35 g / g or more, the absorption capacity of the particulate water-absorbing agent becomes appropriate, and the performance as an absorbent in sanitary products such as disposable diapers is ensured. Furthermore, the upper limit of the CRC (centrifuge retention capacity) of the particulate water-absorbing agent of the present invention is preferably 70 g / g or less, more preferably 60 g / g or less. When the CRC exceeds 70 g / g, gel blocking is likely to occur when the particulate water-absorbing agent swells. Therefore, when the CRC is in an appropriate range, the particulate water-absorbing agent becomes suitable for use in high-absorption-rate disposable diapers and the like. The CRC can be controlled by the type and / or amount of the internal cross-linking agent.

[0070] (2-4) Water Absorption Speed ​​(Vortex Method) The water absorption speed (Vortex method) of the particulate water-absorbing agent of the present invention is preferably 40 seconds or less, more preferably 38 seconds or less, even more preferably 35 seconds or less, particularly preferably 33 seconds or less, and even particularly preferably 31 seconds or less. By improving the SRC (NP) and SEC (4.83 kPa) to the above-mentioned ranges and further controlling the water absorption speed (Vortex method) to the above-mentioned range, the amount of absorption in a short time can be further increased, and the performance when used in sanitary articles such as disposable diapers can be improved.

[0071] (2-5) Surface Tension (STR) Surface tension is the work (free energy) required to increase the surface area of ​​a solid and / or liquid, expressed per unit area. The surface tension referred to in the present application refers to the surface tension of an aqueous solution when a particulate water-absorbing agent is dispersed in a 0.90 mass % sodium chloride aqueous solution. The surface tension is measured by the following procedure. That is, 50 ml of physiological saline adjusted to 20°C and a 25 mm-long fluororesin rotor that has been thoroughly washed are placed in a 100 ml beaker that has been thoroughly washed. Next, the surface tension of the physiological saline is measured using a surface tensiometer (K11 automatic surface tensiometer manufactured by KRUSS), and it is confirmed that the value of the surface tension is 71 to 75 [mN / m]. Subsequently, 0.5 g of the particulate water-absorbing agent is placed in the beaker containing the physiological saline adjusted to 20°C after the surface tension measurement, and the mixture is stirred at 500 rpm for 4 minutes. After 4 minutes, the stirring is stopped, and after the water-containing particulate water-absorbing agent has settled, the surface tension of the supernatant liquid is measured again by the same operation. Note that, in one embodiment of the present invention, a plate method using a platinum plate is adopted, and the plate is thoroughly washed with deionized water and heated and washed with a gas burner before each measurement.

[0072] The surface tension of the particulate water-absorbing agent of the present invention is preferably 66 [mN / m] or more, more preferably 68 [mN / m] or more, even more preferably 70 [mN / m] or more, even more preferably 71 [mN / m] or more, and particularly preferably 72 [mN / m] or more. When the surface tension satisfies the above-mentioned conditions, the amount of wet-back in the sanitary product such as a diaper can be further reduced. An upper limit of the surface tension of 75 [mN / m] is usually sufficient.

[0073] (2-6) Particle Shape The particle shape of the water absorbent resin (powder) is preferably an irregularly pulverized shape. Here, the term "irregularly pulverized shape" refers to particles in a pulverized state that do not have a uniform shape. Compared to spherical particles obtained by reverse phase suspension polymerization or gas phase polymerization, the irregularly pulverized particles are preferable for the following reasons (i) to (iii).

[0074] (i) Irregularly shaped particles have a large surface area and therefore a large contact area with the liquid, resulting in a high absorption rate. (ii) Since irregularly shaped particles do not have a uniform shape, gaps tend to form between the particles, which increases the liquid retention capacity of the gaps formed between the particles, thereby increasing the absorption amount.

[0075] (iii) The irregularly pulverized particles have no fixed shape, and therefore have excellent mixability with hydrophilic fibers such as pulp, and have high liquid diffusibility due to the gaps between the particles.

[0076] The particulate water-absorbing agent according to one embodiment of the present invention is preferably a pulverized product of aqueous polymerization. The irregularly pulverized particles can be obtained by pulverizing a gel or a dried product (preferably a dried product) of a crosslinked polymer obtained through aqueous polymerization. On the other hand, spherical particles or granulated spherical particles obtained without a pulverization step, typically by reverse-phase suspension polymerization or droplet polymerization in which a polymerization monomer is sprayed and polymerized, are not irregularly pulverized. When the particulate water-absorbing agent has an irregularly pulverized shape, the particulate water-absorbing agent is superior to particulate water-absorbing agents with a high average circularity (e.g., spherical ones) in one or more physical properties selected from the group consisting of water absorption rate, SRC (NP), and SRC (4.83 kPa). In one embodiment of the present invention, the average circularity of the particulate water-absorbing agent is preferably 0.70 or less, more preferably 0.60 or less, and even more preferably 0.55 or less.

[0077] The average circularity is calculated, for example, by the following method. 100 or more particulate water absorbing agents are randomly selected, and each particulate water absorbing agent is photographed with an electron microscope (VE-9800 manufactured by Keyence Corporation) (magnification: 50 times) to obtain an image of the particulate water absorbing agent, and the perimeter and area of ​​each particle are calculated using the attached image analysis software. Then, the area and the perimeter are used to calculate the following formula: Circularity = 4 × π × area / (perimeter) 2 The circularity of each particle is determined by the above method, and the average value of the obtained values ​​is calculated as the average circularity.

[0078] (2-7) Inorganic colloid particles, water-insoluble inorganic particles, water-soluble polyvalent metal cation-containing compound From the viewpoint of suppressing adhesion between particles of the water absorbing agent, it is preferable that the particulate water absorbing agent according to one embodiment of the present invention further contains at least one selected from the group consisting of inorganic colloid particles, water-insoluble inorganic particles, and water-soluble polyvalent metal cation-containing compound.

[0079] When the particulate water-absorbing agent of the present invention contains any one of inorganic colloid particles, water-insoluble inorganic particles, and a water-soluble polyvalent metal cation-containing compound, it has excellent handleability in a humid environment. Therefore, by using such a particulate water-absorbing agent, when producing a thin absorbent body for a sanitary product, problems such as the occurrence of aggregation and clogging in the transfer pipes of a production plant and the inability to mix uniformly with hydrophilic fibers can be reduced. Therefore, using such a particulate water-absorbing agent is preferable because it can suppress the performance degradation of the sanitary product when producing the thin absorbent body containing the particulate water-absorbing agent of the present invention.

[0080] The particulate water-absorbing agent can further improve its performance by containing inorganic colloidal particles. The inorganic colloidal particles refer to inorganic particles dispersed in a dispersion medium in a colloidal solution. Specific examples of the inorganic colloidal particles include colloidal silica in which silicon dioxide particles are dispersed in water and alumina sol in which aluminum oxide is dispersed in water. The content of the inorganic colloidal particles is preferably 0.001 to 5 parts by weight, and more preferably 0.01 to 1 part by weight, in terms of solid content, relative to 100 parts by weight of the polyacrylic acid (salt)-based water-absorbing resin in the particulate water-absorbing agent of the present invention.

[0081] The particulate water absorbing agent contains water-insoluble inorganic particles, which can further improve the performance of the particulate water absorbing agent.

[0082] The water-insoluble inorganic particles are not particularly limited, and specific examples of the water-insoluble inorganic particles include silicon dioxide (silica), aluminum hydroxide, zinc oxide, talc, zeolite, hydrotalcite, and tricalcium phosphate.

[0083] The content of the water-insoluble inorganic particles is preferably 0.01% by weight or more and less than 10% by weight, more preferably 0.1 to 5% by weight, based on 100% by weight of the polyacrylic acid (salt)-based water-absorbing resin.

[0084] By incorporating a water-soluble polyvalent metal cation-containing compound into the particulate water-absorbing agent of the present invention, the performance of the particulate water-absorbing agent can be improved.

[0085] The water-soluble polyvalent metal cation-containing compound refers to a compound that contains a divalent or higher, preferably a trivalent or higher, metal cation and is water-soluble. The water-soluble polyvalent metal cation compound is not particularly limited. Specific examples of the water-soluble polyvalent metal cation compound include aluminum chloride, potassium zirconium carbonate, zirconium sulfate, aluminum sulfate, potassium aluminum sulfate, and sodium aluminum sulfate.

[0086] In this specification, "water-soluble" refers to the property of being soluble (or easily soluble) in water at room temperature (20 to 25°C) and under normal pressure (1 atmosphere), for example, the property of dissolving 1 g or more in 100 ml of water at room temperature and normal pressure. In addition, in this specification, "water-insoluble" refers to the property of being insoluble (or poorly soluble) in water at room temperature (20 to 25°C) and under normal pressure (1 atmosphere), for example, the property of dissolving less than 1 g in 100 ml of water at room temperature and normal pressure. The water-insoluble property preferably refers to the property of dissolving less than 0.1 g in 100 ml of water at room temperature and normal pressure.

[0087] The content of the water-soluble polyvalent metal cation-containing compound is preferably 0.001 to 5 parts by weight, more preferably 0.01 to 2 parts by weight, and even more preferably 0.01 to 1 part by weight, in terms of the amount of polyvalent metal cations relative to 100 parts by weight of the polyacrylic acid (salt)-based water absorbent resin. When the content is within these ranges, the performance of the particulate water absorbent can be improved.

[0088] (2-8) Chelating Agent The particulate water-absorbing agent of the present invention preferably further contains at least one chelating agent for the purpose of preventing coloration and deterioration. The chelating agent may be at least one selected from the group consisting of organophosphorus chelating agents and aminocarboxylic acid chelating agents. The particulate water-absorbing agent that has absorbed urine deteriorates over time due to trace amounts of metal ions and L-ascorbic acid contained in the urine, resulting in a decrease in its liquid-retaining capacity, which may lead to the re-extrusion of absorbed liquid from the sanitary article. By including a chelating agent in the particulate water-absorbing agent, it is possible to suppress liquid return over time when the particulate water-absorbing agent is used in a sanitary article.

[0089] The content of the chelating agent is preferably 0 to 3 parts by weight, more preferably 0.005 to 1 part by weight, and even more preferably 0.01 to 0.5 parts by weight, relative to 100 parts by weight of the polyacrylic acid (salt)-based water absorbent resin.

[0090] Furthermore, as the chelating agent, for example, the compounds disclosed in “[2] Chelating Agents” of WO 2011 / 040530 and the amounts used thereof can be applied to one embodiment of the present invention.

[0091] [3] Manufacturing Method of Particulate Water Absorbing Agent Hereinafter, manufacturing steps (3-1) to (3-8) of a particulate water absorbing agent according to one embodiment of the present invention will be described.

[0092] (3-1) Step of preparing aqueous monomer solution This step is a step of preparing an aqueous solution containing acrylic acid (salt) as a monomer as a main component (hereinafter referred to as "aqueous monomer solution"). Note that, although a slurry liquid of the monomer can also be used within a range in which the water absorption performance of the obtained water absorbent resin is not reduced, for convenience, in this section, an aqueous monomer solution will be described.

[0093]

[0113] In addition, the "main component" means that the amount (content) of use of acrylic acid (salt) is usually 50 mol% or more, preferably 70 mol% or more, and more preferably 90 mol% or more (upper limit: 100 mol%) with respect to the whole of monomers (excluding an internal crosslinking agent) to be subjected to a polymerization reaction of a water absorbent resin.

[0094] (Acrylic Acid) In one embodiment of the present invention, from the viewpoint of the physical properties and productivity of the particulate water-absorbing agent to be obtained, acrylic acid and / or a salt thereof (hereinafter referred to as "acrylic acid (salt)") is used as a monomer.

[0095] The "acrylic acid" may be a known acrylic acid. The "acrylic acid" may contain, as a polymerization inhibitor, preferably a methoxyphenol, more preferably p-methoxyphenol, preferably at 200 ppm or less, more preferably 10 to 160 ppm, and even more preferably 20 to 100 ppm. The content of the polymerization inhibitor is preferable from the viewpoint of the polymerizability of the acrylic acid and / or the color tone of the particulate water-absorbing agent. Furthermore, with regard to impurities in acrylic acid, the compounds described in U.S. Patent Application Publication No. 2008 / 0161512 are also applicable to one embodiment of the present invention.

[0096] The "acrylate" is obtained by neutralizing the acrylic acid with the following basic composition. The acrylate may be a commercially available acrylate (e.g., sodium acrylate), or may be obtained by neutralizing acrylic acid in a manufacturing plant for the particulate water-absorbing agent.

[0097] (Basic Composition) In one embodiment of the present invention, the term "basic composition" refers to a composition containing a basic compound, such as a commercially available aqueous sodium hydroxide solution.

[0098] Specific examples of the basic compound include carbonates or hydrogencarbonates of alkali metals, hydroxides of alkali metals, ammonia, organic amines, etc. Among these, from the viewpoint of the physical properties of the obtained particulate water-absorbing agent, it is desirable that the basic compound be strongly basic. That is, as the basic compound, hydroxides of alkali metals such as sodium hydroxide, potassium hydroxide, and lithium hydroxide are preferred, and sodium hydroxide is more preferred.

[0099] (Neutralization) In one embodiment of the present invention, neutralization of acrylic acid (before polymerization) or neutralization of a hydrogel crosslinked polymer obtained by crosslinking polymerization of acrylic acid (after polymerization) (hereinafter referred to as "post-neutralization") can be selected or used in combination. In addition, these neutralizations may be performed by either a continuous method or a batch method, and are not particularly limited, but a continuous method is preferred from the viewpoint of production efficiency, etc.

[0100] In addition, the conditions for the neutralization apparatus, neutralization temperature, residence time, etc. described in International Publication No. 2009 / 123197 or U.S. Patent Application Publication No. 2008 / 0194863 are also applied to one embodiment of the present invention.

[0101] In one embodiment of the present invention, the neutralization rate is preferably 10 to 90 mol%, more preferably 40 to 85 mol%, even more preferably 50 to 80 mol%, and particularly preferably 60 to 75 mol%, based on the acid groups of the monomer. If the neutralization rate is less than 10 mol%, the water absorption capacity may be significantly reduced. On the other hand, if the neutralization rate exceeds 90 mol%, a water-absorbent resin with a high water absorption capacity under pressure may not be obtained.

[0102] The neutralization rate is the same in the case of post-neutralization. The neutralization rate of the particulate water-absorbing agent as a final product is also applied to the neutralization rate. For example, a "neutralization rate of 75 mol%" means a mixture of 25 mol% of acrylic acid and 75 mol% of an acrylic acid salt. The mixture may also be referred to as a partially neutralized product of acrylic acid.

[0103] (Other Monomers) In one embodiment of the present invention, the term "other monomers" refers to monomers other than the acrylic acid (salt), and the particulate water-absorbing agent can be produced by using the other monomers in combination with the acrylic acid (salt).

[0104] The other monomer may be a water-soluble or hydrophobic unsaturated monomer, specifically, the compounds described in U.S. Patent Application Publication No. 2005 / 0215734 (excluding acrylic acid) are also applicable to one embodiment of the present invention.

[0105] (Internal Crosslinking Agent) As the internal crosslinking agent used in one embodiment of the present invention, the compounds described in U.S. Patent No. 6,241,928 are also applied to one embodiment of the present invention. Among these, one or more compounds are selected in consideration of reactivity. Depending on the polymerization form and / or the type of polymerization initiator described below, a crosslinked polymer may be obtained without using an internal crosslinking agent, but it is preferable to use at least one internal crosslinking agent.

[0106] The amount of the internal crosslinking agent used is preferably 0.0001 to 10 mol%, more preferably 0.001 to 1 mol%, even more preferably 0.001 to 0.5 mol%, still more preferably 0.005 to 0.1 mol%, and particularly preferably 0.005 to 0.05 mol%, based on the total amount of monomers. By setting the amount used within the above range, a desired water-absorbent resin can be obtained. If the amount used is too small, the gel strength of the resulting water-absorbent resin tends to decrease and the water-soluble content tends to increase. If the amount used is too large, the water absorption capacity of the resulting water-absorbent resin tends to decrease. The "mol %" based on the total amount of monomers refers to the percentage of the number of moles of the internal crosslinking agent relative to the total number of moles of monomers contained in the aqueous monomer solution.

[0107] In one embodiment of the present invention, a method is preferably used in which a predetermined amount of internal cross-linking agent is added to an aqueous monomer solution in advance, and a cross-linking reaction is carried out simultaneously with polymerization. On the other hand, other methods that can be used include a post-cross-linking method in which an internal cross-linking agent is added during and / or after polymerization; a radical cross-linking method using a radical polymerization initiator; and a radiation cross-linking method using active energy rays such as electron beams and ultraviolet rays. These methods can also be used in combination.

[0108] (Other substances added to aqueous monomer solution) In one embodiment of the present invention, from the viewpoint of improving the physical properties of the resulting water-absorbent resin, the following substances can also be added during preparation of the aqueous monomer solution.

[0109] Examples of such substances include hydrophilic polymers such as starch, starch derivatives, cellulose, cellulose derivatives, polyvinyl alcohol, polyacrylic acid (salts), and crosslinked polyacrylic acid (salts). The hydrophilic polymers can be added to the aqueous monomer solution in amounts of preferably 50% by weight or less, more preferably 20% by weight or less, even more preferably 10% by weight or less, and particularly preferably 5% by weight or less (the lower limit is 0% by weight). Additionally, foaming agents such as carbonates, azo compounds, and bubbles, surfactants, chelating agents, α-hydroxycarboxylic acids (salts), and chain transfer agents can be added to the aqueous monomer solution in amounts of preferably 5% by weight or less, more preferably 1% by weight or less, and even more preferably 0.5% by weight or less. The lower limit for the amount of such substances added is 0% by weight. Examples of such chelating agents include diethylenetriaminepentaacetic acid (salts), triethylenetetraminehexaacetic acid (salts), hydroxyethylidene diphosphonic acid (salts), and ethylenediaminetetramethylenephosphonic acid (salts). As the α-hydroxycarboxylic acid (salt), the compounds exemplified in the (3-7) additive addition step described later can be added in the same manner.

[0110] In addition, the substance may be added not only to the aqueous monomer solution but also during the polymerization, or these forms may be used in combination.

[0111] When a water-soluble resin or a water-absorbent resin is used as the hydrophilic polymer, a graft polymer or a water-absorbent resin composition (for example, a starch-acrylic acid polymer, a PVA-acrylic acid polymer, etc.) is obtained. These polymers and water-absorbent resin compositions also fall within the scope of the present invention.

[0112] (Concentration of Monomer Component) In this step, when preparing an aqueous monomer solution, the above-mentioned substances are added. The concentration of the monomer component in the aqueous monomer solution is not particularly limited, and from the viewpoint of the physical properties of the water-absorbent resin, it is preferably 10 to 80 wt %, more preferably 20 to 75 wt %, and even more preferably 30 to 70 wt %.

[0113] When aqueous solution polymerization or reversed-phase suspension polymerization is employed, a solvent other than water may be used in combination as needed. In this case, the type of solvent is not particularly limited.

[0114] The "concentration of the monomer component" is a value calculated by the following formula (3), and the weight of the aqueous monomer solution does not include the weight of the graft component, the water-absorbent resin, and the hydrophobic solvent in the reversed-phase suspension polymerization.

[0115] (Concentration of monomer component (wt %))=(Weight of monomer component) / (Weight of aqueous monomer solution)×100 Formula (3) (3-2) Polymerization Step This step is a step of polymerizing the acrylic acid (salt)-based aqueous monomer solution obtained in the step of preparing the aqueous monomer solution to obtain a hydrogel-like crosslinked polymer (hereinafter referred to as "hydrogel").

[0116] (Polymerization initiator) The polymerization initiator used in one embodiment of the present invention is not particularly limited, as it is appropriately selected depending on the polymerization form, etc. Examples include thermally decomposable polymerization initiators, photodecomposable polymerization initiators, and redox-based polymerization initiators that are used in combination with a reducing agent that promotes the decomposition of these polymerization initiators. Specifically, one or more of the polymerization initiators disclosed in U.S. Pat. No. 7,265,190 are used. Note that, from the viewpoint of the handleability of the polymerization initiator and the physical properties of the particulate water-absorbing agent or water-absorbing resin, preferably a peroxide or an azo compound is used, more preferably a peroxide, and even more preferably a persulfate.

[0117] The amount of the polymerization initiator used is preferably 0.001 to 1 mol %, more preferably 0.001 to 0.5 mol %, based on the monomers, and the amount of the reducing agent used is preferably 0.0001 to 0.02 mol %, based on the monomers.

[0118] Instead of using the polymerization initiator, the polymerization reaction may be carried out by irradiating with active energy rays such as radiation, electron beams, and ultraviolet rays, or these active energy rays and the polymerization initiator may be used in combination.

[0119] (Polymerization form) The polymerization form applicable to the present invention is not particularly limited, but from the viewpoint of water absorption characteristics, ease of polymerization control, etc., preferred are spray droplet polymerization, aqueous solution polymerization, and reversed-phase suspension polymerization, more preferred are aqueous solution polymerization and reversed-phase suspension polymerization, and even more preferred are aqueous solution polymerization. Among these, continuous aqueous solution polymerization is particularly preferred. As continuous aqueous solution polymerization, either continuous belt polymerization or continuous kneader polymerization can be applied.

[0120] As specific polymerization modes, continuous belt polymerization is disclosed in U.S. Pat. Nos. 4,893,999, 6,241,928, U.S. Patent Application Publication No. 2005 / 215734, etc., and continuous kneader polymerization is disclosed in U.S. Pat. Nos. 6,987,151, 6,710,141, etc. By employing these continuous aqueous solution polymerizations, the production efficiency of a water absorbent resin is improved.

[0121] Furthermore, preferred forms of the continuous aqueous solution polymerization include "high-temperature initiated polymerization" and "high-concentration polymerization." "High-temperature initiated polymerization" refers to a form in which polymerization is initiated at a temperature of the aqueous monomer solution of preferably 30°C or higher, more preferably 35°C or higher, even more preferably 40°C or higher, and particularly preferably 50°C or higher (the upper limit is the boiling point). "High-concentration polymerization" refers to a form in which polymerization is carried out at a monomer concentration of preferably 30% by weight or higher, more preferably 35% by weight or higher, even more preferably 40% by weight or higher, and particularly preferably 45% by weight or higher (the upper limit is the saturated concentration). These polymerization forms can also be used in combination.

[0122] In one embodiment of the present invention, the polymerization can be carried out in an air atmosphere, but from the viewpoint of the color tone of the obtained water-absorbent resin, the polymerization may be carried out in an inert gas atmosphere such as nitrogen or argon. In this case, for example, it is preferable to control the oxygen concentration to 1% by volume or less. It is also preferable to replace the dissolved oxygen in the aqueous monomer solution with an inert gas (for example, dissolved oxygen: less than 1 mg / L).

[0123] In one embodiment of the present invention, foam polymerization can also be employed in which polymerization is carried out by dispersing bubbles (particularly the inert gases mentioned above) in an aqueous monomer solution.

[0124] (3-3) Gel Crushing Step This step is a step in which the hydrogel obtained in the polymerization step is crushed using a gel crusher such as a screw extruder (e.g., a kneader or a meat chopper) or a cutter mill to obtain a particulate hydrogel (hereinafter referred to as "particulate hydrogel"). When kneader polymerization is used in the polymerization step, the polymerization step and the gel crushing step are carried out simultaneously. When gas phase polymerization, reverse phase suspension polymerization, or the like is used in the polymerization step and the particulate hydrogel is obtained directly during the polymerization process, the gel crushing step may not be carried out.

[0125] By controlling the gel crushing means (such as a kneader) and the gel crushing energy (GGE), which is one of the gel crushing conditions described later, the SRC (NP) and SRC (4.83 kPa) of the produced particulate water-absorbing agent can be controlled. In this case, the contents disclosed in WO 2011 / 126079 as the gel crushing conditions and form other than the gel crushing energy (GGE) are preferably applied to one embodiment of the present invention.

[0126] (3-4) Drying Step This step is a step of drying the particulate hydrogel obtained in the polymerization step and / or gel crushing step to a desired resin solid content to obtain a dried polymer. The resin solid content is determined from the loss on drying (the weight change when 1 g of the water-absorbent resin is heated at 180°C for 3 hours), and is preferably 80% by weight or more, more preferably 85 to 99% by weight, even more preferably 90 to 98% by weight, and particularly preferably 92 to 97% by weight.

[0127] The method for drying the particulate hydrogel is not particularly limited, and examples thereof include heat drying, hot air drying, reduced pressure drying, fluidized bed drying, infrared drying, microwave drying, drum dryer drying, drying by azeotropic dehydration with a hydrophobic organic solvent, high-humidity drying using high-temperature water vapor, etc. Among these, from the viewpoint of drying efficiency, hot air drying is preferred, and band drying in which hot air drying is performed on a ventilated belt is more preferred.

[0128] The drying temperature (hot air temperature) in the hot air drying is preferably 120 to 250°C, more preferably 150 to 200°C, from the viewpoint of the color tone of the water-absorbent resin and drying efficiency. Drying conditions other than the drying temperature, such as the hot air speed and drying time, may be appropriately set depending on the water content, total weight, and target resin solid content of the particulate hydrogel to be dried. When band drying is performed, the conditions described in WO 2006 / 100300, WO 2011 / 025012, WO 2011 / 025013, WO 2011 / 111657, etc. are appropriately applied.

[0129] (3-5) Pulverization step, classification step This step is a step of pulverizing the dried polymer obtained in the drying step (pulverization step), and adjusting the particle size to a predetermined range (classification step), to obtain a water absorbent resin powder (for convenience, a powdery water absorbent resin before surface crosslinking is referred to as a "water absorbent resin powder").

[0130] Examples of equipment used in the pulverization step in one embodiment of the present invention include high-speed rotary pulverizers such as roll mills, hammer mills, screw mills, and pin mills, vibration mills, knuckle-type pulverizers, and cylindrical mixers. These may be used in combination as necessary.

[0131] Furthermore, the particle size adjustment method in the classification step in one embodiment of the present invention is not particularly limited, and examples thereof include sieve classification using a JIS standard sieve (JIS Z8801-1 (2000)), air flow classification, etc. Note that the particle size adjustment of a water absorbent resin is not limited to the pulverization step and the classification step, and can be appropriately carried out in a polymerization step (particularly, reverse phase suspension polymerization or spray droplet polymerization) or other steps (for example, a granulation step, a fine powder recovery step).

[0132] The weight average particle diameter (D50) of the water absorbent resin powder obtained in the above step (the water absorbent resin powder before the surface cross-linking step, the so-called base polymer) is preferably 200 to 600 μm, more preferably 200 to 550 μm, even more preferably 250 to 500 μm, and particularly preferably 300 to 500 μm. Furthermore, the proportion of particles having a particle diameter of less than 150 μm in the water absorbent resin powder is preferably 10% by weight or less, more preferably 5% by weight or less, even more preferably 3% by weight or less, and particularly preferably 1% by weight or less. The proportion of particles having a particle diameter of 850 μm or more in the water absorbent resin powder is preferably 5% by weight or less, more preferably 3% by weight or less, and even more preferably 1% by weight or less. Incidentally, as for the lower limit value of the proportion of these particles, the smaller the better in any case, and 0% by weight is desirable, but it may be about 0.1% by weight. Furthermore, the logarithmic standard deviation (σζ) of the particle size distribution is preferably 0.20 to 0.50, more preferably 0.25 to 0.40, and even more preferably 0.27 to 0.35. When the logarithmic standard deviation (σζ) of the particle size distribution is excessively small, the range of particle sizes that can be used becomes narrow, the efficiency of the pulverization and classification steps decreases significantly, and the productivity of the water absorbent resin powder decreases. Therefore, it is preferable that the water absorbent resin powder in one embodiment of the present invention satisfies the above particle size distribution. Note that these particle sizes are measured using standard sieves in accordance with the measurement method disclosed in U.S. Pat. No. 7,638,570 or EDANA ERT420.2-02.

[0133] The above-mentioned particle size is applied not only to the water absorbent resin after surface cross-linking (hereinafter, for convenience, may be referred to as "water absorbent resin particles") but also to a particulate water absorbing agent as a final product. Therefore, in the water absorbent resin particles, it is preferable to perform a surface cross-linking treatment (surface cross-linking step) so as to maintain the particle size in the above-mentioned range, and it is more preferable to adjust the particle size by providing a particle size regulation step after the surface cross-linking step.

[0134] (3-6) Surface Cross-Linking Step

[0143] This step is a step of providing a portion with higher cross-link density on a surface layer (a portion several tens of µm from the surface of a water absorbent resin powder) of a water absorbent resin powder obtained through the above-mentioned steps, and is composed of a mixing step, a heat treatment step and a cooling step (optional).

[0135] In the surface cross-linking step, a surface-cross-linked water-absorbent resin (water-absorbent resin particles) is obtained by radical cross-linking, surface polymerization, cross-linking reaction with a surface cross-linking agent, etc. on the surface of the water-absorbent resin powder.

[0136] (Surface cross-linking agent) The surface cross-linking agent used in one embodiment of the present invention is not particularly limited, and may be an organic or inorganic surface cross-linking agent. Among them, from the viewpoint of the physical properties of the water-absorbent resin and the handling of the surface cross-linking agent, an organic surface cross-linking agent that reacts with a carboxyl group is preferred. For example, one or more surface cross-linking agents disclosed in U.S. Patent No. 7,183,456 may be used. More specifically, polyhydric alcohol compounds, epoxy compounds, haloepoxy compounds, polyvalent amine compounds or condensates thereof with haloepoxy compounds, oxazoline compounds, oxazolidinone compounds, polyvalent metal salts, alkylene carbonate compounds, cyclic urea compounds, etc. may be used.

[0137] Specific examples of the organic surface cross-linking agent include polyalcohol compounds such as (di-, tri-, tetra-, poly)ethylene glycol, (di-, poly)propylene glycol, 1,3-propanediol, 2,2,4-trimethyl-1,3-pentanediol, (poly)glycerin, 2-butene-1,4-diol, 1,4-butanediol, 1,3-butanediol, 1,5-pentanediol, 1,6-hexanediol, trimethylolpropane, di- or triethanolamine, pentaerythritol, and sorbitol; Epoxy compounds such as ethylene glycol diglycidyl ether, (di, poly)glycerol polyglycidyl ether, and glycidol; oxazoline compounds such as 2-oxazolidone, N-hydroxyethyl-2-oxazolidone, and 1,2-ethylenebisoxazoline; 1,3-dioxolan-2-one (ethylene carbonate), 4-methyl-1,3-dioxolan-2-one, 4,5-dimethyl-1,3-dioxolan-2-one, 4,4-dimethyl-1,3-dioxolan-2-one, and 4-ethyl-1,3-dioxolan-2-one; Alkylene carbonate compounds such as solan-2-one, 4-hydroxymethyl-1,3-dioxolan-2-one, 1,3-dioxan-2-one, 4-methyl-1,3-dioxan-2-one, 4,6-dimethyl-1,3-dioxan-2-one, and 1,3-dioxopan-2-one; haloepoxy compounds such as epichlorohydrin, epibromohydrin, and α-methylepichlorohydrin, and polyamine adducts thereof (for example, Hercules Kaimen; registered trademark); γ-glycidoxypropyltrimethoxysilane; Examples include silane coupling agents such as γ-aminopropyltriethoxysilane; oxetane compounds such as 3-methyl-3-oxetanemethanol, 3-ethyl-3-oxetanemethanol, 3-butyl-3-oxetanemethanol, 3-methyl-3-oxetaneethanol, 3-ethyl-3-oxetaneethanol, 3-butyl-3-oxetaneethanol, 3-chloromethyl-3-methyloxetane, 3-chloromethyl-3-ethyloxetane, and polyvalent oxetane compounds; and cyclic urea compounds such as 2-imidazolidinone.

[0138] The polyhydric alcohol is preferably a polyhydric alcohol having 2 to 8 carbon atoms, more preferably a polyhydric alcohol having 3 to 6 carbon atoms, and even more preferably a polyhydric alcohol having 3 or 4 carbon atoms. Furthermore, diols are particularly preferred as the polyhydric alcohol. Examples of diols include ethylene glycol, propylene glycol, 1,3-propanediol, and 1,4-butanediol. Of these, the polyhydric alcohol is preferably one or more polyhydric alcohols selected from propylene glycol (1,2-propanediol), 1,3-propanediol, and 1,4-butanediol.

[0139] The epoxy compound is preferably a polyglycidyl compound, and ethylene glycol diglycidyl ether is preferably used.

[0140]

[0063] In addition to the organic surface crosslinking agent, from the viewpoint of more effectively performing surface crosslinking, a polyvalent cationic polymer such as a polyamine polymer and / or a water-soluble polyvalent metal cation-containing compound may be used in combination as an ion-binding surface crosslinking agent. The water-soluble polyvalent metal cation-containing compound is as described above. These polyvalent cationic polymers and / or water-soluble polyvalent metal cation-containing compounds may be added to a surface crosslinking agent solution described later and mixed with a water absorbent resin powder, or may be added to a water absorbent resin powder separately from the surface crosslinking agent solution and mixed.

[0141]

[0073] The amount of the surface crosslinking agent used (when a plurality of agents are used, the total amount used) is preferably 0.01 to 10 parts by weight, more preferably 0.01 to 5 parts by weight, relative to 100 parts by weight of a water absorbent resin powder. Further, the surface crosslinking agent is preferably added as an aqueous solution, and in this case, the amount of water used is preferably 0.1 to 20 parts by weight, more preferably 0.5 to 10 parts by weight, relative to 100 parts by weight of a water absorbent resin powder. Furthermore, when a hydrophilic organic solvent is used as necessary, the amount used is preferably 10 parts by weight or less, more preferably 5 parts by weight or less, relative to 100 parts by weight of a water absorbent resin powder.

[0142]

[0111] (Mixing Step) This step is a step of mixing a water absorbent resin powder and the surface crosslinking agent. A method of mixing the surface crosslinking agent is not particularly limited, and includes a method of preparing a surface crosslinking agent solution in advance, and mixing the liquid with the water absorbent resin powder, preferably by spraying or dropping, more preferably by spraying.

[0143] The device for carrying out the mixing is not particularly limited, but is preferably a high-speed stirring mixer, more preferably a high-speed stirring continuous mixer.

[0144] (Heat Treatment Step) This step is a step in which heat is applied to the mixture discharged from the mixing step to cause a crosslinking reaction on the surface of the water absorbent resin powder.

[0145] The apparatus for carrying out the crosslinking reaction is not particularly limited, and preferably includes a paddle dryer. The reaction temperature in the crosslinking reaction is appropriately set depending on the type of surface crosslinking agent used, and is preferably 50 to 300°C, more preferably 80 to 200°C.

[0146] (Cooling Step) This step is an optional step that is performed as necessary after the heat treatment step.

[0147] The cooling device is not particularly limited, and is preferably a device with the same specifications as the device used in the heat treatment step, more preferably a paddle dryer. This is because the device can be used as a cooling device by changing the heat medium to a refrigerant. The water-absorbent resin particles obtained in the heat treatment step are forcibly cooled, as necessary, to preferably 40 to 80°C, more preferably 50 to 70°C in the cooling step.

[0148]

[0123] (3-7) Additive Addition Step This step is a step of adding an additive such as a polyvalent metal salt, a cationic polymer, a chelating agent, an inorganic reducing agent, a hydroxycarboxylic acid compound, a water-insoluble inorganic particle, an inorganic colloid particle, a water-soluble polyvalent metal cation-containing compound, a surfactant, a non-polymeric water-soluble compound, etc. to the water absorbent resin particles obtained in the surface crosslinking step. The additive can also be mixed with the water absorbent resin powder simultaneously with the surface crosslinking agent (aqueous solution).

[0149] (Polyvalent Metal Salt and / or Cationic Polymer) From the viewpoint of improving the water absorption rate, liquid permeability, moisture absorption fluidity, etc. of the obtained particulate water-absorbing agent, a polyvalent metal salt and / or a cationic polymer may be added to the water absorbent resin particles obtained in the surface cross-linking step.

[0150] Specific examples of the polyvalent metal salt and / or cationic polymer that can be used in one embodiment of the present invention include compounds disclosed in “[7] Polyvalent metal salt and / or cationic polymer” of WO 2011 / 040530 and the amounts used thereof.

[0151] (Chelating Agent) From the viewpoint of color tone (prevention of coloration) and prevention of deterioration of the resulting particulate water-absorbing agent, a chelating agent may be added to the water-absorbing resin particles obtained in the surface cross-linking step.

[0152] As the chelating agent, for example, the compounds disclosed in “[2] Chelating Agents” of WO 2011 / 040530 and the amounts used thereof are applicable to one embodiment of the present invention.

[0153] (Inorganic Reducing Agent) From the viewpoint of color tone (prevention of coloration), prevention of deterioration, reduction of residual monomers, etc. of the obtained particulate water absorbing agent, an inorganic reducing agent may be added to the water absorbent resin particles obtained in the surface cross-linking step.

[0154] As the inorganic reducing agent, for example, the compounds disclosed in “(3) Inorganic Reducing Agents” of WO 2011 / 040530 and the amounts used thereof are applicable to one embodiment of the present invention.

[0155] (α-Hydroxycarboxylic Acid Compound) From the viewpoint of color tone (prevention of coloration) of the obtained particulate water absorbing agent, etc., α-hydroxycarboxylic acid may be added to the water absorbent resin particles obtained in the surface cross-linking step. Note that the "α-hydroxycarboxylic acid compound" refers to a carboxylic acid having a hydroxyl group in the molecule or a salt thereof, and is a hydroxycarboxylic acid having a hydroxyl group at the α-position.

[0156] As the α-hydroxycarboxylic acid compound, for example, the compounds disclosed in “[6] α-hydroxycarboxylic acid compounds” in WO 2011 / 040530 and the amounts used thereof are applicable to one embodiment of the present invention, and malic acid (salt) and lactic acid (salt) are particularly preferred.

[0157] (Water-insoluble inorganic particles) From the viewpoint of improving the flowability of the particulate water-absorbing agent, water-insoluble inorganic particles may be added to the water-absorbent resin particles obtained in the surface cross-linking step. Examples of the water-insoluble inorganic particles added to the water-absorbent resin particles obtained in the surface cross-linking step include the water-insoluble inorganic particles described in the section (2-6) above.

[0158] (Inorganic colloid particles) From the viewpoint of improving the physical properties of the obtained particulate water-absorbing agent, inorganic colloid particles may be added to the water-absorbent resin particles obtained in the surface cross-linking step. Examples of the inorganic colloid particles added to the water-absorbent resin particles obtained in the surface cross-linking step include the inorganic colloid particles described in the section (2-6) above.

[0159] (Water-soluble polyvalent metal cation-containing compound) From the viewpoint of improving the performance of the obtained particulate water-absorbing agent, a water-soluble polyvalent metal cation-containing compound may be added to the water-absorbent resin particles obtained in the surface cross-linking step. Examples of the water-soluble polyvalent metal cation-containing compound include the water-soluble polyvalent metal cation-containing compounds described in the section (2-6) above.

[0160] (Surfactant) From the viewpoint of improving the physical properties (for example, water absorption rate) of the obtained water absorbent resin, a surfactant may be added to the water absorbent resin particles obtained in the surface cross-linking step.

[0161] Examples of the surfactant include surfactants disclosed in International Publication No. 97 / 017397 or U.S. Pat. No. 6,107,358, i.e., nonionic surfactants, anionic surfactants, cationic surfactants, amphoteric surfactants, and the like.

[0162]

[0044] (Non-polymer water-soluble compound) From the viewpoint of reducing dust of the water absorbent resin, etc., a non-polymer water-soluble compound may be added to the water absorbent resin particles obtained in the surface cross-linking step. As the non-polymer water-soluble compound, for example, the compounds disclosed in "Non-polymer water-soluble compounds" of WO 2014 / 034667 and the amounts used thereof are applicable to one embodiment of the present invention.

[0163] In one embodiment of the present invention, additives other than the additives described above can also be added to the water absorbent resin particles obtained in the surface cross-linking step in order to impart various functions to the water absorbent resin. Examples of the additives include compounds having phosphorus atoms, oxidizing agents, organic reducing agents, organic powders such as metal soaps, deodorants, antibacterial agents, pulp, and thermoplastic fibers.

[0164] The amount of the additive used (added amount) is not particularly limited, as it is determined appropriately depending on the application. The amount used (added amount) is preferably 3 parts by weight or less, more preferably 1 part by weight or less, relative to 100 parts by weight of the water-absorbent resin. In addition, the additive can also be added in a step separate from the above step.

[0165] (3-8) Other Steps In one embodiment of the present invention, in addition to the steps described above, a granulation step, a sizing step, a fine powder removal step, a fine powder recycling step, etc. can be provided as necessary. Furthermore, one or more steps such as a transportation step, a storage step, a packaging step, and a preservation step may be further included. The "sizing step" includes a fine powder removal step subsequent to the surface cross-linking step, and a step of classifying and pulverizing the water-absorbent resin when it aggregates and exceeds a desired size. Furthermore, the "fine powder recycling step" includes a form in which the fine powder is added as it is as in the present invention, as well as a step of making the fine powder into a large hydrogel and adding it to any step in the production process of the water-absorbent resin.

[0166] (3-9) Method for controlling SRC (NP) and SRC (4.83 kPa) By employing the control method described below in the above-described production steps (3-1) to (3-8), the SRC (NP) and SRC (4.83 kPa) of the particulate water-absorbing agent to be produced can be controlled within a preferred range. This allows the particulate water-absorbing agent of the present invention to be suitably produced.

[0167] Examples of the control method include carrying out the gel crushing described in the section "(3-3) Gel Crushing Step" under specific conditions. Specifically, the gel crushing is carried out by controlling the gel crushing energy (GGE) to preferably 15 to 40 J / g, more preferably 20 to 40 J / g, even more preferably 20 to 35 J / g, and particularly preferably 25 to 35 J / g. By carrying out the gel crushing in this manner, the gel crushing can be carried out while applying appropriate shear force and compressive force to the hydrogel. As a result, the particle shape and particle size distribution of the hydrogel can be controlled, and the SRC (NP) and SRC (4.83 kPa) of the produced particulate water-absorbing agent can be controlled within the preferred ranges described above.

[0168] Here, "gel grinding energy" in one embodiment of the present invention refers to the unit energy required by the gel grinding device when grinding a hydrogel, i.e., the mechanical energy per unit mass of the hydrogel. The energy required to heat and cool the jacket and the energy required for the water and steam introduced are not included in the gel grinding energy. Note that "gel grinding energy" is abbreviated as "GGE" from the English term "Gel Grinding Energy."

[0169] When the gel grinder is driven by three-phase AC power, GGE is calculated by the following formula (6): GGE [J / g] = {√3 × voltage × current × power factor × motor efficiency} / {mass of hydrogel fed into the gel grinder per second} ... formula (6) The "power factor" and "motor efficiency" are values ​​specific to the gel grinder that vary depending on the operating conditions, etc., and take values ​​of 0 or more and 1 or less. These values ​​can be obtained by contacting the device manufacturer, etc. In addition, when the gel grinder is driven by single-phase AC power, GGE can be calculated by changing "√3" in formula (6) to "1". The unit of voltage is [V], the unit of current is [A], and the unit of hydrogel mass is [g / s].

[0170] The "power factor" and "motor efficiency" in the GGE are values ​​used during gel crushing. The values ​​of the power factor and motor efficiency during idle operation are approximately defined as in the above formula (6), since the current value during idle operation is small. In the above formula (6), the "mass of hydrogel fed into the gel crusher per second" [g / s] refers to a value converted to [g / s], for example, when the hydrogel is continuously supplied by a metering feeder. However, the hydrogel may contain recycled granulated gel, as described below.

[0171] In addition, in the present invention, the mechanical energy applied to the hydrogel is important. Therefore, it is preferable to calculate the gel crushing energy using the current value obtained by subtracting the current value when the gel crushing device is running idle from the current value during gel crushing as the value of "current" in the formula (6). In particular, when gel crushing is performed using multiple devices, the total current value during idle operation becomes large. Therefore, a method of calculating GGE using the value obtained by subtracting the current value during idle operation from the current value during gel crushing as the value of "current" in the formula (6) is preferable.

[0172] In the present invention, the hydrogel is crushed in the gel crushing step by applying a high GGE of 15 J / g or more, and the CRC of the water-absorbent resin particles obtained by performing the drying step and the crushing and classification step described above after the gel crushing step is preferably 50 to 70 g / g, more preferably 50 to 65 g / g, even more preferably 51 to 63 g / g, and particularly preferably 52 to 62 g / g. However, it is very difficult to control the CRC of the water-absorbent resin particles obtained by crushing the hydrogel with a high GGE of 15 J / g or more, and performing the drying step and the crushing and classification step described above after the gel crushing step within the preferred range. The reason for this is as follows.

[0173] In order to increase the CRC of the water-absorbent resin particles, the hydrogel obtained in the polymerization step must be a low-crosslinked gel with a relatively low crosslinking density. Such a low-crosslinked gel is difficult to pulverize by applying a high GGE of 15 J / g or more. Therefore, it is difficult to apply appropriate shear force and compression force to the low-crosslinked gel to control the SRC (NP) and SRC (4.83 kPa) within the aforementioned preferred range.

[0174] The inventors of the present invention have conducted extensive research into this issue and have succeeded in reducing the dischargeability of the hydrogel from the crusher compared to conventional methods. Methods for reducing the dischargeability of the hydrogel include installing a weir at the crusher outlet, reducing the size of the crusher outlet, and adjusting the perforated plate installed at the crusher outlet. This makes it easier to apply energy to the low-crosslinked gel, even if the hydrogel supplied to the crusher is a low-crosslinked gel, and allows appropriate shear and compressive forces to be applied to the low-crosslinked gel. As a result, the SRC (NP) and SRC (4.83 kPa) were improved.

[0175] In addition, when gel crushing is performed using multiple devices, such as using a screw extruder after kneader polymerization or using multiple screw extruders, the total energy consumed in each device is defined as the gel crushing energy (GGE).

[0176] In addition to the method of performing gel pulverization under the specific conditions described above, other examples of the control method include a method of foaming the water-absorbent resin particles and a method of polymerizing the water-absorbent resin particles by reducing the monomer concentration in the aqueous monomer solution during the polymerization step. By forming the water-absorbent resin particles into a foamed shape, the surface area of ​​the particles can be increased, thereby improving the liquid retention of the particulate water-absorbing agent. Furthermore, by employing the method of polymerizing the particles by reducing the monomer concentration, the performance of the particulate water-absorbing agent can be improved. As a result, the SRC (NP) and SRC (4.83 kPa) of the produced particulate water-absorbing agent can be controlled within the preferred ranges described above.

[0177] [4] Uses of the particulate water absorbing agent The particulate water absorbing agent of the present invention is used for purposes of absorbing water, and is widely used as an absorbent. Furthermore, the particulate water absorbing agent of the present invention can be used in an absorbent article including the absorbent. In particular, the particulate water absorbing agent of the present invention reduces liquid return under pressure, and therefore, among absorbent articles, it is suitably used as a sanitary article for absorbing body fluids such as urine and blood used by humans.

[0178] That is, a preferred embodiment of the present invention is an absorbent body containing the particulate water-absorbing agent of the above-mentioned form. Also, another preferred embodiment of the present invention is a sanitary article containing the absorbent body. Since the absorbent body contains the particulate water-absorbing agent of the present invention, the sanitary article containing the absorbent body can further reduce the return of absorbed liquid during actual use.

[0179] The absorbent body may be an absorbent material formed primarily from a particulate water-absorbing agent and a fibrous base material (e.g., hydrophilic fibers). The content (core concentration) of the particulate water-absorbing agent relative to the total weight of the particulate water-absorbing agent and hydrophilic fibers in the absorbent body is preferably 10 to 100% by weight, more preferably 15 to 90% by weight, particularly preferably 20 to 80% by weight, and most preferably 25 to 80% by weight. The higher the core concentration in the absorbent body, the more the water absorption performance of the absorbent body and sanitary products containing the absorbent body is affected by the water absorption performance of the particulate water-absorbing agent contained in the absorbent body and sanitary products. The particulate water-absorbing agent contained in the absorbent body and sanitary products is the particulate water-absorbing agent used in the production of the absorbent body and sanitary products. Such absorbent bodies are formed, for example, by blending or sandwiching a fibrous base material such as hydrophilic fibers with a particulate water-absorbing agent. Examples of the fiber substrate that can be used include hydrophilic fibers such as pulverized wood pulp, cotton linters, crosslinked cellulose fibers, rayon, cotton, wool, acetate, vinylon, etc. These fiber substrates are preferably air-laid.

[0180] The absorbent body may also be a (pulpless) water-absorbent sheet in which a water-absorbent resin is fixed between two sheets (for example, nonwoven fabric).

[0181] The absorbent article comprises the absorber, a liquid-permeable top sheet, and a liquid-impermeable back sheet. The absorbent article is prepared by manufacturing an absorber (absorbent core) and sandwiching the absorbent core between a liquid-permeable top sheet and a liquid-impermeable back sheet. Thereafter, an elastic member, a diffusion layer, an adhesive tape, etc. are provided as necessary to obtain an absorbent article such as an adult disposable diaper or a sanitary napkin. The absorbent core has a density of, for example, 0.06 to 0.50 [g / cm 3 ], basis weight 0.01 to 0.20 [g / cm 2 ] range.

[0182] An embodiment of the present invention may include the following inventions [1] to [8].

[0183] [1] A particulate water-absorbing agent containing, as a main component, a surface-crosslinked polyacrylic acid (salt)-based water-absorbing resin, which satisfies the following formula (A) and formula (B): SRC(NP)>50.0 g / g (A) SRC(4.83 kPa)>41.5 g / g (B) wherein the SRC(NP) is measured by a method including the following steps (a) to (c):

[0184] (a) The particulate water-absorbing agent (W 0 ) [g] is brought into contact with a 0.9% aqueous sodium chloride solution (hereinafter referred to as the "test liquid") for 10 minutes without applying a load, to obtain a swollen gel.

[0185] (b) separating the swollen gel obtained in step (a) from the test liquid;

[0186] (c) The weight (W) of the swollen gel separated in step (b) 1 ) [g], and calculate the SRC (NP) of the particulate water-absorbing agent based on the following formula (1); SRC (NP) [g / g] = W 1 / W 0 (1) The SRC (4.83 kPa) is measured by carrying out a method including steps (c') to (e') described below in place of step (c) in the method including steps (a) to (c).

[0187] (c') A load of 4.83 kPa is applied to the swollen gel separated in step (b) for 1 minute.

[0188] (d') The exudate exuded from the swollen gel in step (c') is removed.

[0189] (e') The weight (W 2 ) [g] is measured, and the SRC (4.83 kPa) is calculated based on the following formula (2); SRC (4.83 kPa) [g / g] = W 2 / W 0 (2) [2] The particulate water-absorbing agent according to [1], wherein the value of SRC (4.83 kPa) in the formula (B) is greater than 42 g / g.

[0190] [3] The particulate water-absorbing agent according to [1] or [2], wherein the value of SRC(NP) in the formula (A) is >54.

[0191] [4] The particulate water-absorbing agent according to any one of [1] to [3], which has a water absorption speed (Vortex method) of 40 seconds or less.

[0192] [5] The particulate water-absorbing agent according to any one of [1] to [4], which has a surface tension (STR) of 66 mN / m or more.

[0193] [6] The particulate water-absorbing agent according to any one of [1] to [5], which has a centrifuge retention capacity (CRC) of 35 g / g or more.

[0194] [7] The particulate water-absorbing agent according to [6], which has a centrifuge retention capacity (CRC) of 40 g / g or more.

[0195] [8] The particulate water-absorbing agent according to any one of [1] to [7], further comprising at least one selected from the group consisting of inorganic colloid particles, water-insoluble inorganic particles, and water-soluble polyvalent metal cation-containing compounds.

[0196] [9] An absorbent body comprising the particulate water-absorbing agent according to any one of [1] to [8].

[0197]

[10] A hygiene product comprising the absorbent body according to [9].

[0198] The present invention will be described in more detail using the following examples and comparative examples. However, the technical scope of the present invention is not limited to the following examples. In the following examples, unless otherwise specified, the operations were carried out under the conditions of room temperature (20-25°C) and relative humidity 45-55% RH.

[0199] Unless otherwise noted, the electrical equipment used in the Examples, Comparative Examples and Reference Examples (including the measurement of the physical properties of the particulate water-absorbing agent) was powered by a 200V or 100V power supply.

[0200] (a) Measurement Method of SRC (NP) Measurement of SRC (NP) was carried out using a cylinder and a piston used in a Gel Bed Permeability test described in U.S. Patent Publication No. 8269060. A 400-mesh wire netting was attached to the bottom of the cylinder, which was capable of preventing the particulate water-absorbing agent and swollen gel described below from falling out and capable of absorbing or discharging a test liquid and exudate described below.

[0201] First, the total weight of the cylinder and the piston used to measure SRC(NP) is measured, and the value is designated as W a Subsequently, about 0.9 g of a sample of the particulate water-absorbing agent to be measured was weighed out and uniformly spread on the bottom surface of the cylinder. Here, the exact weight of the sample was determined as W 0 Subsequently, the cylinder was placed in a large excess of a 0.9% aqueous sodium chloride solution adjusted to 23±1° C. as a test liquid. The uniformly sprayed sample was brought into contact with the test liquid for 10 minutes, and the sample was allowed to absorb the test liquid and swell without applying a load, thereby obtaining a swollen gel.

[0202] Next, a piston (approximately 72 g) was placed on the swollen gel in the cylinder, and the cylinder was lifted out of the test solution. The cylinder lifted out of the test solution was placed on a JIS standard sieve with a mesh size of 2000 μm. When the cylinder was lifted out of the test solution and placed on the JIS standard sieve, the solution present in the cylinder that was not retained by the swollen gel, i.e., the excess liquid, was drained from the bottom of the cylinder. In other words, the excess liquid that was not retained by the swollen gel was removed.

[0203] The cylinder was left standing on the JIS standard sieve for 1 minute to remove excess water from the swollen gel particles. That is, at the start of the draining, i.e., 1 minute after the cylinder was placed on the JIS standard sieve, no water droplets fell from the measuring device for 5 seconds. Thereafter, the weights of the cylinder, the swollen gel, and the piston were measured. At this time, if water droplets were attached to the bottom and / or side of the cylinder, the water droplets were removed with Kimwipes (S-200, manufactured by Nippon Paper Crecia) or the like before measuring the weight. The weight of the obtained cylinder, the swollen gel, and the piston was calculated as W b [g]. 0 , W a and W b The SRC (NP) of the particulate water-absorbing agent constituting the sample was calculated based on the following formula (1'). b [g]-W a [g]) is the weight of the swollen gel after being left to stand in the above-mentioned step (b): W 1 [g]. SRC(NP) [g / g] = (W b [g]-W a [g]) / W 0[g] (1') (b) Measurement method of SRC (4.83 kPa) Measurement of SRC (4.83 kPa) was carried out using a cylinder, piston, and weight used in a Gel Bed Permeability test described in U.S. Patent Publication No. 8269060. A 400-mesh wire netting was attached to the bottom of the cylinder, which was capable of preventing the particulate water-absorbing agent and swollen gel described below from falling out and capable of absorbing or discharging a test liquid and exudate described below.

[0204] First, the total weight of the cylinder, piston, and weight used to measure the SRC (4.83 kPa) was measured, and the value was designated as W c Subsequently, about 0.9 g of a sample of the particulate water-absorbing agent to be measured was weighed out and uniformly spread on the bottom surface of the cylinder. Here, the exact weight of the sample was determined as W 0 Subsequently, the cylinder was placed in a large excess of a 0.9% aqueous sodium chloride solution adjusted to 23±1° C. as a test liquid. The uniformly sprayed sample was brought into contact with the test liquid for 10 minutes, and the sample was allowed to absorb the test liquid and swell without applying a load, thereby obtaining a swollen gel.

[0205] Next, a piston (approximately 72 g) was placed on the swollen gel in the cylinder, and the cylinder was lifted out of the test solution. The cylinder lifted out of the test solution was placed on a JIS standard sieve with a mesh size of 2000 μm. When the cylinder was lifted out of the test solution and placed on the JIS standard sieve, the solution present in the cylinder that was not retained by the swollen gel, i.e., the excess liquid, was drained from the bottom of the cylinder. In other words, the excess liquid that was not retained by the swollen gel was removed.

[0206] The cylinder was left on the JIS standard sieve for 1 minute to remove excess water from the swollen gel particles. That is, at the start of the draining, i.e., 1 minute after the cylinder was placed on the JIS standard sieve, no water droplets fell from the measuring device for 5 seconds. The weight (approximately 1,316 g) was then placed on the piston. At this time, the load applied to the swollen gel was 4.83 kPa. This operation caused the solution that had been retained between the swollen gel particles before pressure application to exude. A portion of the exuded solution, i.e., the exudate, seeped out from the bottom of the swollen gel, i.e., onto the bottom of the cylinder, and drained from the bottom. Meanwhile, the remainder of the exudate accumulated above the swollen gel, i.e., on the top of the piston. One minute after the weight was placed on the piston, the exudate stopped leaking and reached a steady state. The remaining exudate that had accumulated on the top of the piston was quickly removed using a dropper. After removing the exudate exuded from the swollen gel as described above, the weights of the cylinder, the piston, the weight, and the swollen gel were measured. At this time, if water droplets were attached to the bottom and / or side of the cylinder, the water droplets were removed using Kimwipes (S-200, manufactured by Nippon Paper Crecia) or the like before measuring the weight. The weight of the cylinder, the piston, the weight, and the swollen gel obtained was calculated as W d [g]. 0 , W c and W d Using the above, the SRC (4.83 kPa) of the particulate water-absorbing agent constituting the sample was calculated based on the following formula (2'). d [g]-W c [g]) is the weight of the swollen gel after removing the exudate in the above-mentioned step (d'): W 2 [g]. SRC(4.83 kPa) [g / g] = (W d [g]-W c [g]) / W 0 [g] (2') (c) Method for Measuring CRC The centrifuge retention capacity (absorption capacity without load, CRC) of the particulate water-absorbing agent or water-absorbing resin was measured in accordance with the EDANA method (ERT441.2-02).

[0207] (d) Particle Size Distribution (Particle Size Distribution, Weight Average Particle Diameter (D50), Logarithmic Standard Deviation (σζ) of Particle Size Distribution) The particle size distribution (particle size distribution, weight average particle diameter (D50), logarithmic standard deviation (σζ) of particle size distribution) of a particulate water-absorbing agent or a water-absorbent resin was measured in accordance with “(3) Mass-Average Particle Diameter (D50) and Logarithmic Standard Deviation (σζ) of Particle Diameter Distribution” described in columns 27 and 28 of U.S. Pat. No. 7,638,570.

[0208] (e) Measurement method of water absorption rate (Vortex method) 0.02 parts by weight of food additive, Blue No. 1, was added to 1000 parts by weight of a previously prepared 0.90 wt% sodium chloride aqueous solution, and the liquid temperature was adjusted to 30 ° C. 50 ml of the blue-colored 0.90 wt% sodium chloride aqueous solution was weighed into a 100 ml beaker, and 2.00 g of a particulate water-absorbing agent was added while stirring at 600 rpm using a cylindrical stirrer with a length of 40 mm and a diameter of 8 mm, and the water absorption time (seconds) was measured. The endpoint was measured in accordance with the standard described in JIS K 7224-1996 "Explanation of the water absorption rate test method for superabsorbent polymers," and the time until the water-absorbing agent absorbed the saline solution and the test liquid covered the stirrer tip was taken as the water absorption rate (seconds).

[0209] (f) Method for measuring surface tension (STR): 50 ml of saline adjusted to 20°C and a 25 mm long fluororesin rotor that had been thoroughly washed were placed in a thoroughly washed 100 ml beaker, and the surface tension of the saline was measured using a surface tensiometer (K11 automatic surface tensiometer manufactured by KRUSS). The surface tension was confirmed to be in the range of 71 to 75 mN / m.

[0210] Next, 0.5 g of the particulate water-absorbing agent was put into a beaker containing the physiological saline solution after the surface tension measurement, which had been adjusted to 20°C, and the mixture was stirred for 4 minutes under the condition of 500 rpm. After 4 minutes, the stirring was stopped, and the water-absorbed particulate water-absorbing agent was allowed to settle, and then the surface tension of the supernatant liquid was measured by the same operation as that for measuring the surface tension of the physiological saline solution alone. In this example, a plate method using a platinum plate was adopted, and the plate was thoroughly washed with deionized water and heated and washed with a gas burner before each measurement.

[0211] (g) Method for Measuring Absorption Amount by Absorbent Body <Preparation of Absorbent Body A> Two 2.8 g absorbent cotton sheets were prepared by uniformly tearing an 80 mm x 160 mm piece of absorbent cotton (cut cotton manufactured by Kawamoto Sangyo Co., Ltd., 8 cm x 16 cm) in the surface direction. Next, absorbent paper was cut into 200 mm x 200 mm pieces, and an 8 cm x 16 cm frame was placed near the center of the cut absorbent paper. One of the absorbent cotton sheets weighing 2.8 g was placed inside the frame, and the upper surface of the absorbent cotton sheet was smoothed with an acrylic plate or the like. 3 g of particulate water-absorbing agent was uniformly dispersed on the upper surface, and the other absorbent cotton sheet weighing 2.8 g was placed on top to form a sand structure. A load of 10 kg was applied to the entire frame, and the frame was maintained for one minute to form an absorbent body. Thereafter, the weight and the frame were removed, and both ends of the water-absorbent paper were folded back along the longitudinal direction of the absorbent body to wrap the absorbent body. The obtained absorbent body was placed in a nonwoven fabric bag (10 cm x 22 cm) made using Heatlon paper, and the periphery was heat-sealed to produce absorbent body A.

[0212] <Measurement of Absorption Amount by Absorbent> A deep tray was filled with 0.9% aqueous sodium chloride solution to a liquid depth of 5 cm or more, and the liquid temperature in the tray was adjusted to 25°C. Absorbent A was immersed in the tray and left for 10 minutes without applying any load, causing absorbent A to swell. After swelling, the swollen absorbent A was removed from the tray while maintaining a horizontal position relative to the liquid surface in the tray, and, while maintaining this horizontal position, placed on a JIS standard sieve with a diameter of 45 cm and a mesh size of 2000 μm. Next, an acrylic plate was placed on a portion of the upper surface of absorbent A having an area of ​​8 cm x 16 cm where the particulate water-absorbing agent was present, and a weight with a total weight of 6405 g together with the acrylic plate was placed on top of the acrylic plate, and the liquid was drained for 1 minute. The pressure applied by the acrylic plate and the weight to the portion of absorbent A on which the acrylic plate was placed was 50 g / cm. 2 The weight of absorbent body A after draining was measured, and the difference between this and the weight of absorbent body A measured before immersion was calculated as the "amount absorbed by the absorbent body." The calculated values ​​are shown in Table 2.

[0213] (h) Method for Measuring the Amount of Liquid Wake-Back from the Absorbent Body <Method for Producing Absorbent Body B> A piece of vinyl tape (Vinyl Tape 21-100TM manufactured by Nitto Denko Corporation) was cut into a size of 100 mm x 200 mm, placed with the adhesive side facing upward, and an 80 mm x 160 mm frame was placed on top of it. An 80 mm x 160 mm piece of absorbent cotton (cut cotton 8 cm x 16 cm manufactured by Kawamoto Sangyo Co., Ltd.) was uniformly torn in the surface direction to prepare a 2.8 g absorbent cotton sheet, which was then placed within the frame. Furthermore, 1.5 g of a particulate water-absorbing agent was uniformly sprayed onto the absorbent cotton sheet within the frame. The frame was removed, and a separately cut piece of air-through nonwoven fabric to a size of 100 mm x 200 mm was placed on top of the particulate water-absorbing agent, and the outer periphery of the air-through nonwoven fabric was attached with vinyl tape to produce absorbent body B.

[0214] <Measurement of Liquid Return Amount from Absorbent> 70 mL of a 0.9% aqueous sodium chloride solution was poured into the center of absorbent B. The sodium chloride solution was poured using a liquid feeder consisting of an 80 mm x 160 mm flat plate with a 20 mm inner diameter circular hole in the center and a cylinder with an inner diameter of 20 mm and a length of 80 mm. The inside of the cylinder was connected to the circular hole. The liquid feeder was placed above the 8 cm x 16 cm portion of the upper surface of absorbent B where the particulate water-absorbing agent was present, i.e., the central portion. Using a funnel with a flow rate of 7 mL / sec, the sodium chloride solution was poured into the center of absorbent B through the cylinder and the circular hole. Ten minutes after the start of the pouring of the aqueous sodium chloride solution, 30 sheets of 80 mm x 80 mm filter paper, the weight of which had been measured in advance, were placed in the central portion, and the entire filter paper was pressed with a 3200 g weight for 1 minute. At this time, liquid seeped out of the absorbent B and was absorbed by the filter paper. The filter paper used was a 100 mm x 100 mm filter paper, Model No. 2, manufactured by ADVANTEC, cut to 80 mm x 80 mm. The difference between the weight of the filter paper before use and the weight of the filter paper after absorbing the liquid was calculated as the "amount of liquid returning from the absorbent." The calculated values ​​are shown in Table 2.

[0215] [Production Example 1] A monomer aqueous solution (1) was prepared containing 300 parts by weight of acrylic acid, 123.6 parts by weight of a 48 wt% aqueous solution of sodium hydroxide, 0.44 parts by weight of polyethylene glycol diacrylate (average n number: 9) (hereinafter referred to as "PEGDA-9"), 1.18 parts by weight of a 31 wt% aqueous solution of ethylenediaminetetramethylenephosphonic acid, and 331.8 parts by weight of deionized water.

[0216] Next, the aqueous monomer solution (1), whose temperature had been adjusted to 41°C, was continuously fed by a metering pump to a continuous polymerizer having a flat polymerization belt equipped with weirs on both ends of the belt, and polymerization was carried out. Prior to feeding into the continuous polymerizer, 127.0 parts by weight of a 48 wt% aqueous sodium hydroxide solution was continuously mixed with the aqueous monomer solution (1) by a line mixer. After mixing, the liquid temperature of the mixture of the aqueous monomer solution (1) and the 48 wt% aqueous sodium hydroxide solution rose to 80°C due to the heat of neutralization.

[0217] The obtained aqueous monomer solution (1) was continuously mixed with 10.6 parts by weight of a 5 wt % aqueous sodium persulfate solution using a line mixer to obtain a mixed solution. The mixed solution was continuously supplied to the continuous polymerizer so that the liquid depth on the polymerization belt was 10 mm. A polymerization reaction occurred on the polymerization belt, and a belt-shaped hydrogel (1) was obtained. The polymerization time was 3 minutes. The obtained belt-shaped hydrogel (1) was continuously cut at equal intervals in the width direction relative to the traveling direction of the polymerization belt so that the cut length was 300 mm, to obtain a hydrogel (1).

[0218] The hydrogel (1) was supplied to a screw extruder, and gel pulverization of the hydrogel (1) was carried out. The screw extruder was a meat chopper having a tip equipped with a perforated plate having a diameter of 100 mm, a hole diameter of 4.0 mm, 207 holes, and a thickness of 10 mm, and an outer diameter of a screw shaft of 86 mm. With the screw shaft rotation speed of the meat chopper set to 130 rpm, the hydrogel (1) was supplied to the meat chopper at 4640 [g / min] and steam at 83 [g / min] simultaneously. Thus, gel pulverization was carried out on the hydrogel (1). As a result, a pulverized gel after gel pulverization, i.e., a particulate hydrogel (1), was obtained. The gel pulverization energy (GGE) in the gel pulverization was 29.3 [J / g].

[0219] The particulate hydrogel (1) was spread on a 50-mesh wire netting and dried with hot air at 180°C for 30 minutes to obtain a dried product A (1). The dried product A (1) was pulverized using a roll mill (WML type roll pulverizer / Inoguchi Giken Co., Ltd.) to obtain a pulverized product (1). The pulverized product (1) was then sieved using JIS sieves with mesh sizes of 850 μm, 600 μm, 500 μm, 300 μm, 150 μm, and 45 μm.

[0220] As a result, irregularly pulverized water-absorbent resin particles (1) were obtained. The physical properties of the water-absorbent resin particles (1) were measured by the above-mentioned method. As a result, the water-absorbent resin particles (1) had a mass-average particle diameter (D50) of 358 μm, a logarithmic standard deviation (σζ) of the particle size distribution of 0.36, and a centrifuge retention capacity (CRC) of 53.4 (g / g).

[0221] [Production Example 2] Instead of 0.44 parts by weight of PEGDA-9, 0.36 parts by weight of polyethylene glycol diacrylate having an average n number of 4 was used. Furthermore, instead of 1.18 parts by weight of a 31 wt% ethylenediaminetetramethylenephosphonic acid aqueous solution, 0.82 parts by weight of a 45 wt% diethylenetriaminepentaacetic acid aqueous solution was used. Except for these, irregularly pulverized water-absorbent resin particles were obtained by the same method as in Production Example 1. The water-absorbent resin particles are designated as water-absorbent resin particles (2). The gel-crushing energy (GGE) in the gel-crushing of Production Example 2 was 27.9 [J / g]. The physical properties of the water-absorbent resin particles (2) were measured by the above-mentioned method. As a result, the water-absorbent resin particles (2) had a mass-average particle diameter (D50) of 337 μm, a logarithmic standard deviation (σζ) of the particle size distribution of 0.34, and a centrifuge retention capacity (CRC) of 56.1 (g / g).

[0222] [Production Example 3] The amount of PEGDA-9 used was changed to 0.52 parts by weight. In addition, 1.83 parts by weight of a 1 wt% diethylenetriamine pentaacetic acid aqueous solution was used instead of 1.18 parts by weight of a 31 wt% ethylenediaminetetramethylenephosphonic acid aqueous solution. Furthermore, the amount of deionized water used was changed to 332.9 parts by weight. Except for these, irregularly pulverized water-absorbent resin particles were obtained by the same method as in Production Example 1. The water-absorbent resin particles are referred to as water-absorbent resin particles (3). The gel-crushing energy (GGE) in the gel crushing of Production Example 3 was 31.1 [J / g]. The physical properties of the water-absorbent resin particles (3) were measured by the above-mentioned method. As a result, the water-absorbent resin particles (3) had a mass-average particle diameter (D50) of 346 μm, a logarithmic standard deviation (σζ) of the particle size distribution of 0.35, and a centrifuge retention capacity (CRC) of 51.1 (g / g).

[0223] [Production Example 4] Irregularly pulverized water-absorbent resin particles were obtained by the same method as in Production Example 1, except that the hole diameter of the perforated plate at the tip of the screw extruder was changed to 9.5 mm and the number of holes to 40. The water-absorbent resin particles were designated as water-absorbent resin particles (4). The gel-crushing energy (GGE) in the gel-crushing of Production Example 4 was 8.3 [J / g]. The physical properties of the water-absorbent resin particles (4) were measured by the above-mentioned method. As a result, the water-absorbent resin particles (4) had a mass-average particle diameter (D50) of 341 μm, a logarithmic standard deviation (σζ) of the particle size distribution of 0.34, and a centrifuge retention capacity (CRC) of 53.7 (g / g).

[0224] [Production Example 5] Irregularly pulverized water-absorbent resin particles were obtained by the same method as in Production Example 2, except that the hole diameter of the perforated plate at the tip of the screw extruder was changed to 9.5 mm and the number of holes to 40. The water-absorbent resin particles were designated as water-absorbent resin particles (5). The gel-crushing energy (GGE) in the gel-crushing of Production Example 5 was 7.2 [J / g]. The physical properties of the water-absorbent resin particles (5) were measured by the above-mentioned method. As a result, the water-absorbent resin particles (5) had a mass-average particle diameter (D50) of 353 μm, a logarithmic standard deviation (σζ) of the particle size distribution of 0.36, and a centrifuge retention capacity (CRC) of 56.3 (g / g).

[0225] [Production Example 6] Irregularly pulverized water-absorbent resin particles were obtained by the same method as in Production Example 3, except that the hole diameter of the perforated plate at the tip of the screw extruder was changed to 9.5 mm and the number of holes to 40. The water-absorbent resin particles were designated as water-absorbent resin particles (6). The gel-crushing energy (GGE) in the gel-crushing of Production Example 6 was 9.8 [J / g]. The physical properties of the water-absorbent resin particles (6) were measured by the above-mentioned method. As a result, the water-absorbent resin particles (6) had a mass-average particle diameter (D50) of 338 μm, a logarithmic standard deviation (σζ) of the particle size distribution of 0.34, and a centrifuge retention capacity (CRC) of 50.9 (g / g).

[0226] [Production Example 7] Water-absorbent resin particles (7) were produced by citing Example 12-1 of WO 2017 / 170605.

[0227] [Production Example 8] Water-absorbent resin particles (8) were produced by citing Example 1-13 of WO 2021 / 201177.

[0228] [Production Example 9] Irregularly pulverized water absorbent resin particles (9) were obtained by the same method as in Production Example 1, except for the following changes. The amount of PEGDA-9 used was changed to 0.63 parts by weight. In addition, 1.83 parts by weight of a 1% by weight aqueous solution of diethylenetriaminepentaacetic acid was used instead of 1.18 parts by weight of a 31% by weight aqueous solution of ethylenediaminetetramethylenephosphonic acid. Furthermore, 1.83 parts by weight of a 60% by weight aqueous solution of sodium lactate was added as a raw material for the aqueous monomer solution (1), and the amount of deionized water used was changed to 328.3 parts by weight.

[0229] The gel crushing energy (GGE) in the gel crushing of Production Example 9 was 29.0 [J / g]. The physical properties of the water-absorbent resin particles (9) were measured by the above-mentioned method. The water-absorbent resin particles (9) had a mass average particle diameter (D50) of 350 μm, a logarithmic standard deviation (σζ) of the particle size distribution of 0.37, and a centrifuge retention capacity (CRC) of 53.1 (g / g).

[0230] [Production Example 10] Irregularly pulverized water absorbent resin particles (10) were obtained by the same method as in Production Example 1, except for the following changes. The amount of PEGDA-9 used was changed to 0.50 parts by weight. In addition, 1.83 parts by weight of a 1% by weight aqueous solution of diethylenetriaminepentaacetic acid was used instead of 1.18 parts by weight of a 31% by weight aqueous solution of ethylenediaminetetramethylenephosphonic acid. Furthermore, 2.93 parts by weight of a 50% by weight aqueous solution of malic acid was added as a raw material for the aqueous monomer solution (1), and the amount of deionized water used was changed to 327.1 parts by weight.

[0231] The gel crushing energy (GGE) in the gel crushing of Production Example 10 was 28.1 [J / g]. The physical properties of the water-absorbent resin particles (10) were measured by the above-mentioned method. The water-absorbent resin particles (10) had a mass average particle diameter (D50) of 342 μm, a logarithmic standard deviation (σζ) of the particle size distribution of 0.36, and a centrifuge retention capacity (CRC) of 54.0 (g / g).

[0232] [Example 1] A surface crosslinking agent solution was uniformly mixed with the water absorbent resin particles (1) obtained in Production Example 1, and then the obtained mixture was heat-treated at 190°C for 30 minutes to obtain a water absorbent resin (1). The surface crosslinking agent solution was a solution containing 0.025 parts by weight of ethylene glycol diglycidyl ether, 0.3 parts by weight of ethylene carbonate, 0.5 parts by weight of propylene glycol, and 2.0 parts by weight of deionized water relative to 100 parts by weight of the water absorbent resin particles (1).

[0233] Thereafter, 30 g of the cooled water-absorbent resin (1) was placed in a glass container having a diameter of 6 cm and a height of 11 cm, and the container was placed in a paint shaker (No. 488 test disperser, manufactured by Toyo Seiki Seisakusho, Ltd.). Next, the paint shaker was shaken at 800 (cycles / min) for 30 minutes. Thereafter, an EDTMP·5Na aqueous solution was uniformly mixed with the shaken water-absorbent resin (1) relative to 100 parts by weight of the water-absorbent resin (1). The EDTMP·5Na aqueous solution was an aqueous solution consisting of 1 part by weight of water and 0.01 part by weight of sodium salt of ethylenediaminetetramethylenephosphonic acid (EDTMP·5Na) when the weight of the water-absorbent resin (1) was taken as 100 parts by weight.

[0234] Subsequently, an aqueous solution consisting of 1.0 part by weight of water, 1.0 part by weight of propylene glycol, and 1.5 parts by weight of an aqueous cationic colloidal silica solution relative to 100 parts by weight of the water absorbent resin (1) was uniformly mixed with the water absorbent resin (1) mixed with the EDTMP.5Na aqueous solution. The aqueous cationic colloidal silica solution is a trade name: Klebosol 30CAL25 30% aqueous solution, manufactured by AZ Electronic Material, Inc. / aluminum cation-containing silicon dioxide fine particles.

[0235] The obtained mixture was dried at 60°C for 1 hour, and then passed through a JIS standard sieve with an opening of 850 µm to obtain a particulate water-absorbing agent (1). The physical properties of the particulate water-absorbing agent (1) were measured using the above-mentioned methods. The results are shown in Table 2 below.

[0236] [Example 2] A particulate water-absorbing agent (2) was obtained by carrying out the same operation as in Example 1, except for the following points. As a surface cross-linking agent solution, a solution consisting of 0.025 parts by weight of ethylene glycol diglycidyl ether, 0.31 parts by weight of 1,4-butanediol, 0.5 parts by weight of propylene glycol, and 2 parts by weight of deionized water was used, relative to 100 parts by weight of the water-absorbent resin particles (2). Instead of the EDTMP·5Na aqueous solution, an aqueous solution consisting of 1 part by weight of water, 0.03 parts by weight of EDTMP·5Na, and 0.05 parts by weight of sodium hydrogen sulfite was used. Instead of the aqueous solution consisting of 1.0 part by weight of water, 1.0 part by weight of propylene glycol, and 1.5 parts by weight of a cationic colloidal silica aqueous solution, a solution consisting of 1.0 part by weight of water and 1.5 parts by weight of an alumina sol aqueous solution was used.

[0237] The physical properties of the particulate water-absorbing agent (2) were measured using the above-mentioned methods. The results are shown in the following Table 2. The alumina sol aqueous solution used was a trade name of Aluminasol 520-A (a 20.5% aqueous solution of aluminum oxide, manufactured by Nissan Chemical Industries, Ltd.).

[0238] [Example 3] A particulate water-absorbing agent (3) was obtained by carrying out the same operation as in Example 1, except for the following points. As the surface cross-linking agent solution, a solution consisting of 0.02 parts by weight of ethylene glycol diglycidyl ether, 1.3 parts by weight of propylene glycol, and 3.2 parts by weight of deionized water was used, relative to 100 parts by weight of the water-absorbent resin particles (1). The mixture obtained by uniformly mixing the water-absorbent resin particles (1) and the surface cross-linking agent was heat-treated at 100°C for 40 minutes, instead of heat-treating at 190°C for 30 minutes. The shaking time of the paint shaker was changed from 30 minutes to 10 minutes. Instead of the EDTMP·5Na aqueous solution, a polyethylene glycol aqueous solution consisting of 1 part by weight of water and 0.03 parts by weight of polyethylene glycol (average molecular weight 400) was used. Without using an aqueous solution consisting of 1.0 part by weight of water, 1.0 part by weight of propylene glycol, and 1.5 parts by weight of an aqueous cationic colloidal silica solution, the mixture of the polyethylene glycol aqueous solution and the water-absorbent resin was dried at 60° C. for 1 hour, and then passed through a JIS standard sieve with an opening of 850 μm. After passing through the JIS standard sieve, 0.3 parts by weight of silicon dioxide (product name: Aerosil 200, manufactured by Nippon Aerosil Co., Ltd.) was further mixed uniformly.

[0239] The physical properties of the particulate water-absorbing agent (3) were measured using the above-mentioned methods, and the results are shown in Table 2 below.

[0240] [Example 4] A particulate water-absorbing agent (4) was obtained by carrying out the same operation as in Example 1, except for the following points. As the surface cross-linking agent solution, a solution consisting of 0.02 parts by weight of ethylene glycol diglycidyl ether, 1.8 parts by weight of propylene glycol, 2.7 parts by weight of deionized water, and 0.5 parts by weight of aluminum sulfate 14-18 hydrate was used, relative to 100 parts by weight of the water-absorbent resin particles (1). The mixture obtained by uniformly mixing the water-absorbent resin particles (1) and the surface cross-linking agent was heat-treated at 100°C for 40 minutes, instead of at 190°C for 30 minutes. The shaking time of the paint shaker was changed from 30 minutes to 10 minutes. Instead of the EDTMP.5Na aqueous solution, a polyethylene glycol aqueous solution consisting of 1 part by weight of water, 0.12 parts by weight of polyethylene glycol (average molecular weight 600), and 0.03 parts by weight of sodium sulfite was used. Without using an aqueous solution containing 1.0 part by weight of water, 1.0 part by weight of propylene glycol, and 1.5 parts by weight of an aqueous solution of cationic colloidal silica, a mixture of the polyethylene glycol aqueous solution and a water absorbent resin was dried at 60°C for 1 hour, and then passed through a JIS standard sieve having an opening of 850 µm.

[0241] The physical properties of the particulate water-absorbing agent (4) were measured using the above-mentioned methods, and the results are shown in Table 2 below.

[0242] [Example 5] A particulate water-absorbing agent (5) was obtained by carrying out the same operation as in Example 1, except for the following points. As a surface cross-linking agent solution, a solution consisting of 0.025 parts by weight of ethylene glycol diglycidyl ether, 0.26 parts by weight of 1,3-propanediol, 0.5 parts by weight of propylene glycol, and 2 parts by weight of deionized water was used, relative to 100 parts by weight of the water-absorbent resin particles (1). Instead of the EDTMP.5Na aqueous solution, a polyethylene glycol aqueous solution consisting of 1 part by weight of water and 0.1 parts by weight of polyethylene glycol (average molecular weight 400) was used. Instead of the aqueous solution consisting of 1.0 part by weight of water, 1.0 part by weight of propylene glycol, and 1.5 parts by weight of a cationic colloidal silica aqueous solution, an aluminum sulfate aqueous solution consisting of 1.5 parts by weight of water and 0.5 parts by weight of aluminum sulfate 14-18 hydrate was used.

[0243] The physical properties of the particulate water-absorbing agent (5) were measured using the above-mentioned methods, and the results are shown in Table 2 below.

[0244] Example 6 A particulate water-absorbing agent (6) was obtained by carrying out the same operation as in Example 1, except for the following points. Instead of the water-absorbent resin particles (1), the water-absorbent resin particles (2) prepared in Production Example 2 were used. Instead of the EDTMP-5Na aqueous solution, a DTPA-3Na aqueous solution consisting of 2.0 parts by weight of water, 0.02 parts by weight of diethylenetriaminepentaacetic acid trisodium (DTPA-3Na), and 0.1 parts by weight of sodium sulfite was used. Without using an aqueous solution consisting of 1.0 part by weight of water, 1.0 part by weight of propylene glycol, and 1.5 parts by weight of a cationic colloidal silica aqueous solution, the mixture of the DTPA-3Na aqueous solution and the water-absorbent resin was dried at 60°C for 1 hour and then passed through a JIS standard sieve with an opening of 850 μm. After passing through the JIS standard sieve, 0.3 parts by weight of hydrotalcite (trade name: DHT-6, manufactured by Kyowa Chemical Industry Co., Ltd.) was further mixed uniformly.

[0245] The physical properties of the particulate water-absorbing agent (6) were measured using the above-mentioned methods, and the results are shown in Table 2 below.

[0246] [Example 7] A particulate water-absorbing agent (7) was obtained by performing the same operation as in Example 1, except for the following points. Instead of the water-absorbent resin particles (1), the water-absorbent resin particles (2) prepared in Production Example 2 were used. As the surface-crosslinking agent solution, a solution consisting of 0.02 parts by weight of ethylene glycol diglycidyl ether, 1.8 parts by weight of propylene glycol, and 2.7 parts by weight of deionized water was used, relative to 100 parts by weight of the water-absorbent resin particles (2). The mixture obtained by uniformly mixing the water-absorbent resin particles (2) and the surface-crosslinking agent was heat-treated at 100°C for 40 minutes, instead of at 190°C for 30 minutes. The shaking time of the paint shaker was changed from 30 minutes to 10 minutes. Instead of the EDTMP·5Na aqueous solution, a sodium hydrogen sulfite aqueous solution consisting of 0.5 parts by weight of water and 0.03 parts by weight of sodium hydrogen sulfite was used. Instead of an aqueous solution consisting of 1.0 part by weight of water, 1.0 part by weight of propylene glycol, and 1.5 parts by weight of an aqueous cationic colloidal silica solution, a solution consisting of 1.0 part by weight of water, 1.0 part by weight of propylene glycol, and 1.5 parts by weight of an aqueous alumina sol solution was used.

[0247] The physical properties of the particulate water-absorbing agent (7) were measured using the above-mentioned methods. The results are shown in the following Table 2. The alumina sol aqueous solution used was a trade name of Aluminasol 520-A (a 20.5% aqueous solution of aluminum oxide, manufactured by Nissan Chemical Industries, Ltd.).

[0248] [Example 8] A particulate water-absorbing agent (8) was obtained by performing the same operation as in Example 1, except for the following points. - The water-absorbent resin particles (2) prepared in Production Example 2 were used instead of the water-absorbent resin particles (1). - As a surface-crosslinking agent solution, a solution consisting of 0.025 parts by weight of ethylene glycol diglycidyl ether, 0.31 parts by weight of 1,4-butanediol, 0.5 parts by weight of propylene glycol, and 2 parts by weight of deionized water was used relative to 100 parts by weight of the water-absorbent resin particles (2). - The shaking time of the paint shaker was changed from 30 minutes to 10 minutes. - Without using an EDTMP.5Na aqueous solution, a mixture of a water-absorbent resin and an aqueous solution consisting of 1.0 part by weight of water, 1.0 part by weight of propylene glycol, and 1.5 parts by weight of an aqueous cationic colloidal silica solution was dried at 60°C for 1 hour, and then passed through a JIS standard sieve with an opening of 850 μm.

[0249] The physical properties of the particulate water absorbing agent (8) were measured using the above-mentioned methods, and the results are shown in Table 2 below.

[0250] [Example 9] A particulate water-absorbing agent (9) was obtained by carrying out the same operation as in Example 1, except for the following points. - The water-absorbent resin particles (1) were replaced with the water-absorbent resin particles (2) prepared in Production Example 2. - The EDTMP-5Na aqueous solution was replaced with a DTPA-3Na aqueous solution composed of 1.5 parts by weight of water and 0.01 parts by weight of diethylenetriaminepentaacetic acid trisodium (DTPA-3Na). - The aqueous solution composed of 1.0 part by weight of water, 1.0 part by weight of propylene glycol, and 1.5 parts by weight of a cationic colloidal silica aqueous solution was replaced with an aluminum sulfate aqueous solution composed of 1.5 parts by weight of water, 1.0 part by weight of propylene glycol, and 0.5 parts by weight of aluminum sulfate 14-18 hydrate.

[0251] The physical properties of the particulate water-absorbing agent (9) were measured using the above-mentioned methods, and the results are shown in Table 2 below.

[0252] [Example 10] A particulate water-absorbing agent (10) was obtained by carrying out the same operation as in Example 1, except for the following points. Instead of the water-absorbent resin particles (1), the water-absorbent resin particles (2) prepared in Production Example 2 were used. Instead of the EDTMP-5Na aqueous solution, a mixed solution consisting of 2.0 parts by weight of water, 0.01 parts by weight of diethylenetriaminepentaacetic acid-trisodium (DTPA-3Na), 0.05 parts by weight of sodium sulfite, and 0.03 parts by weight of polyethylene glycol (average molecular weight 600) was used. Without using an aqueous solution consisting of 1.0 part by weight of water, 1.0 part by weight of propylene glycol, and 1.5 parts by weight of an aqueous cationic colloidal silica solution, a mixture of the mixed solution and the water-absorbent resin was dried at 60°C for 1 hour and then passed through a JIS standard sieve with an opening of 850 μm. After passing through a JIS standard sieve, 0.3 parts by weight of silicon dioxide (product name: Reolosil QS-20, manufactured by Tokuyama Corporation) was further mixed uniformly.

[0253] The physical properties of the particulate water-absorbing agent (10) were measured using the above-mentioned methods, and the results are shown in Table 2 below.

[0254] [Example 11] A particulate water-absorbing agent (11) was obtained by carrying out the same operation as in Example 1, except for the following points. - The water-absorbent resin particles (3) prepared in Production Example 3 were used instead of the water-absorbent resin particles (1). - As the surface-crosslinking agent solution, a solution consisting of 0.02 parts by weight of ethylene glycol diglycidyl ether, 2.45 parts by weight of propylene glycol, 3.55 parts by weight of deionized water, and 0.5 parts by weight of aluminum sulfate 14-18 hydrate was used relative to 100 parts by weight of the water-absorbent resin particles (3). - The mixture obtained by uniformly mixing the water-absorbent resin particles (3) and the surface-crosslinking agent was heat-treated at 100°C for 40 minutes, instead of heat-treating at 190°C for 30 minutes. - The shaking time of the paint shaker was changed from 30 minutes to 10 minutes. Instead of the EDTMP·5Na aqueous solution, a DTPA·3Na aqueous solution consisting of 1.5 parts by weight of water, 0.15 parts by weight of polyethylene glycol (average molecular weight 400), and 0.03 parts by weight of diethylenetriaminepentaacetic acid·trisodium (DTPA·3Na) was used. Without using an aqueous solution consisting of 1.0 part by weight of water, 1.0 part by weight of propylene glycol, and 1.5 parts by weight of an aqueous cationic colloidal silica solution, the mixture of the DTPA·3Na aqueous solution and a water-absorbent resin was dried at 60°C for 1 hour and then passed through a JIS standard sieve with an opening of 850 μm.

[0255] The physical properties of the particulate water-absorbing agent (11) were measured using the above-mentioned methods, and the results are shown in Table 2 below.

[0256] [Example 12] A particulate water-absorbing agent (12) was obtained by carrying out the same operation as in Example 1, except for the following points. - The water-absorbent resin particles (3) prepared in Production Example 3 were used instead of the water-absorbent resin particles (1). - As a surface-crosslinking agent solution, a solution consisting of 0.025 parts by weight of ethylene glycol diglycidyl ether, 0.26 parts by weight of 1,3-propanediol, 0.5 parts by weight of propylene glycol, and 2 parts by weight of deionized water was used relative to 100 parts by weight of the water-absorbent resin particles (3). - Instead of the EDTMP·5Na aqueous solution, a mixed solution consisting of 1.5 parts by weight of water, 0.05 parts by weight of polyethylene glycol (average molecular weight 600), 0.05 parts by weight of ethylenediaminetetramethylenephosphonic acid sodium salt (EDTMP·5Na), and 0.1 parts by weight of sodium sulfite was used. Instead of an aqueous solution consisting of 1.0 part by weight of water, 1.0 part by weight of propylene glycol, and 1.5 parts by weight of an aqueous cationic colloidal silica solution, a solution consisting of 1.0 part by weight of water, 1.0 part by weight of propylene glycol, and 1.5 parts by weight of an aqueous alumina sol solution was used.

[0257] The physical properties of the particulate water-absorbing agent (12) were measured using the above-mentioned methods, and the results are shown in Table 2 below.

[0258] [Example 13] A particulate water-absorbing agent (13) was obtained by carrying out the same operation as in Example 1, except for the following points. - The water-absorbent resin particles (1) were replaced with the water-absorbent resin particles (3) prepared in Production Example 3. - As the surface-crosslinking agent solution, a solution consisting of 0.02 parts by weight of ethylene glycol diglycidyl ether, 1.3 parts by weight of propylene glycol, and 3.2 parts by weight of deionized water, relative to 100 parts by weight of the water-absorbent resin particles (3), was used. - The mixture obtained by uniformly mixing the water-absorbent resin particles (3) and the surface-crosslinking agent was heated at 100°C for 40 minutes, instead of being heated at 190°C for 30 minutes. - Instead of the EDTMP-5Na aqueous solution, a DTPA-3Na aqueous solution consisting of 1 part by weight of water and 0.02 parts by weight of diethylenetriaminepentaacetic acid trisodium (DTPA-3Na) was used. Instead of an aqueous solution consisting of 1.0 part by weight of water, 1.0 part by weight of propylene glycol, and 1.5 parts by weight of an aqueous cationic colloidal silica solution, an aqueous solution consisting of 1.0 part by weight of water and 1.5 parts by weight of an aqueous cationic colloidal silica solution was used.

[0259] The physical properties of the particulate water-absorbing agent (13) were measured using the above-mentioned methods, and the results are shown in Table 2 below.

[0260] [Comparative Example 1] A comparative particulate water-absorbing agent (1) was produced in the same manner as in Example 1, except that the water-absorbing resin particles (4) prepared in Production Example 4 were used instead of the water-absorbing resin particles (1). The physical properties of the comparative particulate water-absorbing agent (1) were measured using the above-mentioned methods. The results are shown in Table 2 below.

[0261] [Comparative Example 2] A comparative particulate water-absorbing agent (2) was produced in the same manner as in Example 3, except that the water-absorbing resin particles (4) prepared in Production Example 4 were used instead of the water-absorbing resin particles (1). The physical properties of the comparative particulate water-absorbing agent (2) were measured using the above-mentioned methods. The results are shown in Table 2 below.

[0262] [Comparative Example 3] A comparative particulate water-absorbing agent (3) was produced in the same manner as in Example 5, except that the water-absorbing resin particles (4) prepared in Production Example 4 were used instead of the water-absorbing resin particles (1). The physical properties of the comparative particulate water-absorbing agent (3) were measured using the above-mentioned methods. The results are shown in Table 2 below.

[0263] [Comparative Example 4] A comparative particulate water-absorbing agent (4) was produced in the same manner as in Example 6, except that the water-absorbing resin particles (5) prepared in Production Example 5 were used instead of the water-absorbing resin particles (2). The physical properties of the comparative particulate water-absorbing agent (4) were measured using the above-mentioned methods. The results are shown in Table 2 below.

[0264] [Comparative Example 5] A comparative particulate water-absorbing agent (5) was produced in the same manner as in Example 9, except that the water-absorbing resin particles (5) prepared in Production Example 5 were used instead of the water-absorbing resin particles (2). The physical properties of the comparative particulate water-absorbing agent (5) were measured using the above-mentioned methods. The results are shown in Table 2 below.

[0265] [Comparative Example 6] A comparative particulate water-absorbing agent (6) was produced in the same manner as in Example 12, except that the water-absorbing resin particles (6) prepared in Production Example 6 were used instead of the water-absorbing resin particles (3). The physical properties of the comparative particulate water-absorbing agent (6) were measured using the above-mentioned methods. The results are shown in Table 2 below.

[0266] [Comparative Example 7] A comparative particulate water-absorbing agent (7) was produced by the same operation as in Example 7 of WO 2017 / 170605. The physical properties of the comparative particulate water-absorbing agent (7) were measured using the above-mentioned method. The results are shown in Table 2 below.

[0267] [Comparative Example 8] A comparative particulate water-absorbing agent (8) was produced by the same operation as in Example 12-1 of WO 2017 / 170605. The physical properties of the comparative particulate water-absorbing agent (8) were measured using the above-mentioned method. The results are shown in Table 2 below.

[0268] [Comparative Example 9] A comparative particulate water-absorbing agent (9) was produced by performing the same operation as in Example 1-13 of WO 2021 / 201177. The physical properties of the comparative particulate water-absorbing agent (9) were measured using the above-mentioned method. The results are shown in Table 2 below.

[0269] [Example 14] A particulate water-absorbing agent (14) was obtained by performing the same operation as in Example 1, except for the following points. - The water-absorbent resin particles (9) prepared in Production Example 9 were used instead of the water-absorbent resin particles (1). - As the surface-crosslinking agent solution, a solution consisting of 0.025 parts by weight of ethylene glycol diglycidyl ether, 1.8 parts by weight of propylene glycol, and 2.7 parts by weight of deionized water was used relative to 100 parts by weight of the water-absorbent resin particles (9). - The mixture obtained by uniformly mixing the water-absorbent resin particles (9) and the surface-crosslinking agent was heat-treated at 100°C for 40 minutes, instead of heat-treating at 190°C for 30 minutes. - Instead of the EDTMP-5Na aqueous solution, a DTPA-3Na aqueous solution consisting of 1.5 parts by weight of water and 0.02 parts by weight of diethylenetriaminepentaacetic acid trisodium (DTPA-3Na) was used. Instead of an aqueous solution consisting of 1.0 part by weight of water, 1.0 part by weight of propylene glycol, and 1.5 parts by weight of an aqueous cationic colloidal silica solution, an aqueous solution consisting of 1.0 part by weight of water, 1.0 part by weight of propylene glycol, and 1.5 parts by weight of an aqueous alumina sol solution was used.

[0270] The physical properties of the particulate water-absorbing agent (14) were measured using the above-mentioned methods. The results are shown in the following Table 2. The alumina sol aqueous solution used was a trade name of Aluminasol 520-A (a 20.5% aqueous solution of aluminum oxide, manufactured by Nissan Chemical Industries, Ltd.).

[0271] [Example 15] A particulate water-absorbing agent (15) was obtained by carrying out the same operation as in Example 1, except for the following points. - The water-absorbent resin particles (9) prepared in Production Example 9 were used instead of the water-absorbent resin particles (1). - As a surface-crosslinking agent solution, a solution consisting of 0.025 parts by weight of ethylene glycol diglycidyl ether, 0.26 parts by weight of 1,3-propanediol, 0.5 parts by weight of propylene glycol, and 2 parts by weight of deionized water was used relative to 100 parts by weight of the water-absorbent resin particles (9). - Instead of the EDTMP·5Na aqueous solution, a mixed solution consisting of 0.5 parts by weight of water, 0.05 parts by weight of polyethylene glycol (average molecular weight 400), 0.03 parts by weight of a sodium salt of ethylenediaminetetramethylenephosphonic acid (EDTMP·5Na), and 0.05 parts by weight of sodium sulfite was used. Instead of an aqueous solution consisting of 1.0 part by weight of water, 1.0 part by weight of propylene glycol, and 1.5 parts by weight of an aqueous cationic colloidal silica solution, an aqueous solution consisting of 1.5 parts by weight of water, 1.0 part by weight of propylene glycol, and 0.5 parts by weight of aluminum sulfate 14-18 hydrate was used.

[0272] The physical properties of the particulate water-absorbing agent (15) were measured using the above-mentioned methods, and the results are shown in Table 2 below.

[0273] [Example 16] A particulate water-absorbing agent (16) was obtained by performing the same operation as in Example 1, except for the following points. Instead of the water-absorbent resin particles (1), the water-absorbent resin particles (9) prepared in Production Example 9 were used. As the surface-crosslinking agent solution, a solution consisting of 0.02 parts by weight of ethylene glycol diglycidyl ether, 1.3 parts by weight of propylene glycol, and 3.2 parts by weight of deionized water was used, relative to 100 parts by weight of the water-absorbent resin particles (9). The mixture obtained by uniformly mixing the water-absorbent resin particles (9) and the surface-crosslinking agent was heat-treated at 100°C for 40 minutes, instead of at 190°C for 30 minutes. The shaking time of the paint shaker was changed from 30 minutes to 10 minutes. Instead of the EDTMP·5Na aqueous solution, an aqueous solution consisting of 1.5 parts by weight of water, 0.07 parts by weight of ethylenediaminetetramethylenephosphonic acid sodium salt (EDTMP·5Na), and 0.1 parts by weight of sodium sulfite was used. Without using an aqueous solution consisting of 1.0 part by weight of water, 1.0 part by weight of propylene glycol, and 1.5 parts by weight of an aqueous cationic colloidal silica solution, a mixture of the aqueous solution and a water-absorbent resin was dried at 60°C for 1 hour, and then passed through a JIS standard sieve with an opening of 850 µm. After passing through the JIS standard sieve, 0.3 part by weight of hydrotalcite (trade name: DHT-6, manufactured by Kyowa Chemical Industry Co., Ltd.) was further mixed uniformly.

[0274] The physical properties of the particulate water-absorbing agent (16) were measured using the above-mentioned methods, and the results are shown in Table 2 below.

[0275] [Example 17] A particulate water-absorbing agent (17) was obtained by performing the same operation as in Example 1, except for the following points. Instead of the water-absorbent resin particles (1), the water-absorbent resin particles (10) prepared in Production Example 10 were used. As the surface-crosslinking agent solution, a solution consisting of 0.025 parts by weight of ethylene glycol diglycidyl ether, 1.3 parts by weight of propylene glycol, and 3.2 parts by weight of deionized water was used relative to 100 parts by weight of the water-absorbent resin particles (10). Instead of uniformly mixing the water-absorbent resin particles (10) and the surface-crosslinking agent, the mixture was heated at 100°C for 40 minutes, instead of heating at 190°C for 30 minutes. Instead of the EDTMP.5Na aqueous solution, a mixed solution consisting of 1.5 parts by weight of water, 0.03 parts by weight of polyethylene glycol (average molecular weight 600), and 0.05 parts by weight of diethylenetriaminepentaacetic acid trisodium (DTPA.3Na) was used. Instead of an aqueous solution consisting of 1.0 part by weight of water, 1.0 part by weight of propylene glycol, and 1.5 parts by weight of an aqueous cationic colloidal silica solution, an aqueous solution consisting of 1.0 part by weight of water and 1.5 parts by weight of an aqueous cationic colloidal silica solution was used.

[0276] The physical properties of the particulate water-absorbing agent (17) were measured using the above-mentioned methods, and the results are shown in Table 2 below.

[0277] [Example 18] A particulate water-absorbing agent (18) was obtained by performing the same operation as in Example 1, except for the following points. Instead of the water-absorbent resin particles (1), the water-absorbent resin particles (10) prepared in Production Example 10 were used. As the surface-crosslinking agent solution, a solution consisting of 0.02 parts by weight of ethylene glycol diglycidyl ether, 1.8 parts by weight of propylene glycol, and 2.7 parts by weight of deionized water was used, relative to 100 parts by weight of the water-absorbent resin particles (10). A mixture obtained by uniformly mixing the water-absorbent resin particles (10) and the surface-crosslinking agent was heat-treated at 100°C for 40 minutes, instead of at 190°C for 30 minutes. The shaking time of the paint shaker was changed from 30 minutes to 10 minutes. Instead of the EDTMP·5Na aqueous solution, a mixed solution consisting of 2 parts by weight of water, 0.25 parts by weight of polyethylene glycol (average molecular weight 400), and 0.1 parts by weight of diethylenetriaminepentaacetic acid·trisodium (DTPA·3Na) was used. Instead of an aqueous solution consisting of 1.0 part by weight of water, 1.0 part by weight of propylene glycol, and 1.5 parts by weight of an aqueous cationic colloidal silica solution, an aqueous aluminum sulfate solution consisting of 1.5 parts by weight of water and 0.5 parts by weight of aluminum sulfate 14-18 hydrate was used.

[0278] The physical properties of the particulate water-absorbing agent (18) were measured using the above-mentioned methods, and the results are shown in Table 2 below.

[0279] [Example 19] A particulate water-absorbing agent (19) was obtained by carrying out the same operation as in Example 1, except for the following points. - The water-absorbent resin particles (1) were replaced with the water-absorbent resin particles (10) prepared in Production Example 10. - As the surface cross-linking agent solution, a solution containing 0.02 parts by weight of ethylene glycol diglycidyl ether, 1.8 parts by weight of propylene glycol, 2.7 parts by weight of deionized water, and 0.5 parts by weight of aluminum sulfate 14-18 hydrate was used relative to 100 parts by weight of the water-absorbent resin particles (10). - The mixture obtained by uniformly mixing the water-absorbent resin particles (10) and the surface cross-linking agent was heated at 100°C for 40 minutes, instead of being heated at 190°C for 30 minutes. Instead of the EDTMP.5Na aqueous solution, a mixed solution consisting of 2 parts by weight of water, 0.2 parts by weight of polyethylene glycol (average molecular weight 600), 0.07 parts by weight of diethylenetriaminepentaacetic acid.trisodium (DTPA.3Na), and 0.1 parts by weight of sodium sulfite was used. Without using an aqueous solution consisting of 1.0 part by weight of water, 1.0 part by weight of propylene glycol, and 1.5 parts by weight of an aqueous cationic colloidal silica solution, a mixture of the mixed solution and a water-absorbent resin was dried at 60°C for 1 hour and then passed through a JIS standard sieve with an opening of 850 µm.

[0280] The physical properties of the particulate water-absorbing agent (19) were measured using the above-mentioned methods, and the results are shown in Table 2 below.

[0281] Example 20 A particulate water-absorbing agent (20) was obtained by carrying out the same operation as in Example 1, except for the following points. Instead of the water-absorbent resin particles (1), the water-absorbent resin particles (10) prepared in Production Example 10 were used. Instead of the EDTMP·5Na aqueous solution, an aqueous solution consisting of 1 part by weight of water, 0.07 parts by weight of ethylenediaminetetramethylenephosphonic acid sodium salt (EDTMP·5Na), and 0.03 parts by weight of sodium hydrogen sulfite was used. Without using an aqueous solution consisting of 1.0 part by weight of water, 1.0 part by weight of propylene glycol, and 1.5 parts by weight of a cationic colloidal silica aqueous solution, a mixture of the aqueous solution and the water-absorbent resin was dried at 60°C for 1 hour and then passed through a JIS standard sieve with an opening of 850 μm. After passing through the JIS standard sieve, 0.3 parts by weight of silicon dioxide (trade name: Aerosil 200, manufactured by Nippon Aerosil Co., Ltd.) was further mixed uniformly.

[0282] The physical properties of the particulate water-absorbing agent (20) were measured using the above-mentioned methods, and the results are shown in Table 2 below.

[0283] [Comparative Example 10] A surface crosslinking agent solution was uniformly mixed with the water absorbent resin particles (6) obtained in Production Example 6, and then the obtained mixture was heat-treated at 190°C for 30 minutes to obtain a water absorbent resin (1). The surface crosslinking agent solution was a solution containing 0.025 parts by weight of ethylene glycol diglycidyl ether, 0.3 parts by weight of ethylene carbonate, 0.5 parts by weight of propylene glycol and 2.0 parts by weight of deionized water relative to 100 parts by weight of the water absorbent resin particles (1).

[0284] Thereafter, 30 g of the cooled water-absorbent resin (1) was placed in a glass container having a diameter of 6 cm and a height of 11 cm, and the container was placed in a paint shaker (No. 488 test disperser, manufactured by Toyo Seiki Seisaku-sho, Ltd.). Next, the paint shaker was shaken at 800 (cycles / min) for 30 minutes.

[0285] The obtained mixture was dried at 60°C for 1 hour, and then passed through a JIS standard sieve with an opening of 850 µm to obtain a comparative particulate water absorbing agent (10). The physical properties of the comparative particulate water absorbing agent (10) were measured using the above-mentioned methods. The results are shown in Table 2 below.

[0286] [Comparative Example 11] An aluminum sulfate aqueous solution was uniformly mixed with the comparative particulate water absorbing agent (10) obtained in Comparative Example 10. The aluminum sulfate aqueous solution was an aqueous solution containing 1.5 parts by weight of water and 0.5 parts by weight of aluminum sulfate 14-18 hydrate, where the weight of the comparative particulate water absorbing agent (10) was taken as 100 parts by weight.

[0287] The obtained mixture was dried at 60°C for 1 hour, and then passed through a JIS standard sieve with an opening of 850 µm to obtain a comparative particulate water absorbing agent (11). The physical properties of the comparative particulate water absorbing agent (11) were measured using the above-mentioned methods. The results are shown in Table 2 below.

[0288] [Comparative Example 12] The comparative particulate water-absorbing agent (10) obtained in Comparative Example 10 was uniformly mixed with an aqueous solution containing 1 part by weight of water, 0.01 part by weight of diethylenetriaminepentaacetic acid trisodium salt (DTPA 3Na), and 0.004 part by weight of polyoxyethylene sorbitan monostearate (trade name: Rheodol Tw-S120V, manufactured by Kao Corporation).

[0289] Subsequently, an aluminum sulfate aqueous solution was uniformly mixed in. The aluminum sulfate aqueous solution was an aqueous solution containing 1.5 parts by weight of water and 0.5 parts by weight of aluminum sulfate 14-18 hydrate, where the weight of the comparative particulate water absorbing agent (10) was taken as 100 parts by weight.

[0290] The obtained mixture was dried at 60°C for 1 hour, and then passed through a JIS standard sieve with an opening of 850 µm to obtain a comparative particulate water absorbing agent (12). The physical properties of the comparative particulate water absorbing agent (12) were measured using the above-mentioned methods. The results are shown in Table 2 below.

[0291] [Results] The gel grinding energy (GGE) as a production condition in Production Examples 1 to 10 and the physical properties of the water-absorbent resin particles (1) to (10) prepared in Production Examples 1 to 10 are shown in Table 1 below.

[0292] The physical properties of the particulate water absorbing agents (1) to (20) and the comparative particulate water absorbing agents (1) to (12) produced in Examples 1 to 20 and Comparative Examples 1 to 12 are shown below.

[0293] As shown in Table 2, the particulate water-absorbing agents (1) to (20) produced in Examples 1 to 20 have an SRC (NP) of more than 50.0 g / g and an SRC (4.83 kPa) of more than 41.5 g / g. Therefore, the particulate water-absorbing agents (1) to (20) correspond to the particulate water-absorbing agents of the present invention. Furthermore, the particulate water-absorbing agents (1) to (20) are also excellent in water absorption rate (Vortex). On the other hand, the comparative particulate water-absorbing agents (1) to (12) produced in Comparative Examples 1 to 12 have an SRC (NP) of 50.0 g / g or less and / or an SRC (4.83 kPa) of 41.5 or less, and do not correspond to the particulate water-absorbing agents of the present invention.

[0294] Furthermore, the water absorbent bodies using the particulate water absorbing agents (1) to (20) have a larger absorption capacity and a smaller amount of liquid return in the absorbent body compared to the comparative particulate water absorbing agents (1) to (12). In particular, the amount of liquid return in the absorbent body is significantly smaller for the particulate water absorbing agents (1) to (20) than for the comparative particulate water absorbing agent (9) with a low SRC (4.83 kPa) and the comparative particulate water absorbing agent (12) with a low STR. Therefore, the particulate water absorbing agents (1) to (20) can absorb a large amount of 0.9% sodium chloride aqueous solution in a short time because of their high SRC (NP), and because of their high SRC (4.83 kPa), they have excellent liquid retention and reduced liquid return, even when held under high pressure after absorbing liquid.

[0295] From the above, the particulate water-absorbing agent of the present invention has a function of absorbing a large amount of urine in a short time, and also has a function of retaining liquid even when strong external pressure is applied due to the user's movements after absorbing the water. The function is particularly necessary for a particulate water-absorbing agent used in sanitary products such as diapers for adults, which are used in large amounts of urine per urination. As a result, it has been found that the particulate water-absorbing agent of the present invention has an effect of being able to be used in the manufacture of sanitary products that have excellent liquid retention properties in actual use and can further reduce the return of absorbed liquid in actual use.

[0296] The particulate water-absorbing agent according to one embodiment of the present invention can be widely used in the field of sanitary products such as diapers.

Claims

1. A particulate water absorbing agent mainly composed of a surface-crosslinked polyacrylic acid (salt)-based water absorbing resin, which satisfies the following formula (A) and formula (B): SRC(NP)>50.0 g / g (A) SRC(4.83 kPa)>41.5 g / g (B) Here, the SRC(NP) is measured by a method including the following steps (a) to (c). (a) The particulate water absorbing agent (W 0 ) [g] is brought into contact with a 0.9% sodium chloride aqueous solution (hereinafter referred to as the "test liquid") for 10 minutes without applying a load to obtain a swollen gel. (b) The swollen gel obtained in step (a) is separated from the test liquid. (c) The weight (W 1 ) [g], and the SRC (NP) of the particulate water absorbing agent is calculated based on the following formula (1); SRC (NP) [g / g] = W 1 / W 0 (1) The SRC (4.83 kPa) is measured by carrying out a method including steps (c') to (e') described below in place of step (c) in the method including steps (a) to (c). (c') A load of 4.83 kPa is applied to the swollen gel separated in step (b) for 1 minute. (d') The exudate exuded from the swollen gel in step (c') is removed. (e') The weight (W) of the swollen gel obtained in step (d') is measured. 2 ) [g], and the SRC (4.83 kPa) is calculated based on the following formula (2); SRC (4.83 kPa) [g / g] = W 2 / W 0 (2) 2. The particulate water absorbing agent according to claim 1, wherein the value of SRC (4.83 kPa) in the formula (B) is >42 g / g.

3. The particulate water absorbing agent according to claim 1 or 2, wherein the value of SRC(NP) in formula (A) is >54 g / g.

4. The particulate water absorbing agent according to any one of claims 1 to 3, which has a water absorption speed (Vortex method) of 40 seconds or less.

5. The particulate water absorbing agent according to any one of claims 1 to 4, which has a surface tension (STR) of 66 mN / m or more.

6. The particulate water-absorbing agent according to any one of claims 1 to 5, which has a centrifuge retention capacity (CRC) of 35 g / g or more.

7. The particulate water absorbing agent according to claim 6, which has a centrifuge retention capacity (CRC) of 40 g / g or more.

8. The particulate water-absorbing agent according to any one of claims 1 to 7, further comprising at least one member selected from the group consisting of inorganic colloid particles, water-insoluble inorganic particles, and water-soluble polyvalent metal cation-containing compounds.

9. An absorbent comprising the particulate water-absorbing agent according to any one of claims 1 to 8.

10. A sanitary product comprising an absorbent body according to claim 9.

Citation Information

Patent Citations

  • Method for continuous production of water-absorbent resin

    US20050215734A1

  • Production Process of Polyacrylic Acid (Salt) Water-Absorbent Resin

    US20080161512A1

  • Neutralization Process

    US20080194863A1

  • Apparatus for the continuous production of polymers and copolymers of water-soluble monomers

    US4893999A

  • Water-absorbent resin and method for production thereof

    US6107358A

Cited By

  • Water absorbent resin particles, water absorbent body, water absorbent article, and method for producing water absorbent resin particles

    WO2025126867A1