Powdery composition for ceramic molding and method for producing same

The use of cellulose nanofibers and inorganic particles in a specific powder composition for ceramic molding enables high-density filling at low pressure, addressing the energy inefficiencies and void issues in traditional methods, and producing strong ceramic sintered bodies with reduced energy consumption.

WO2024204153A1PCT designated stage expired Publication Date: 2024-10-03DKS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011869
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Ceramic press molding faces challenges in achieving high-density filling under low pressure due to the low fluidity of non-granulated compositions, which is energy-intensive and results in voids and reduced strength in the molded products.

Method used

A powder composition for ceramic molding comprising cellulose nanofibers and inorganic particles with specific size and functional group characteristics, allowing for high-density filling at low pressure without granulation, achieved through spraying or sprinkling a cellulose nanofiber aqueous dispersion onto inorganic particles, eliminating the need for energy-intensive spray drying.

Benefits of technology

The composition exhibits excellent fluidity and high-density filling capabilities, resulting in strong and void-free ceramic sintered bodies with improved strength and reduced energy consumption in the manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

Provided is a powdery composition for ceramic molding that can be easily prepared at low energy and can be packed at a high density even at a low pressure when producing a molded article. A powdery composition for ceramic molding according to an embodiment contains cellulose nanofibers and inorganic particles having an average particle diameter of from 0.005 μm to 2 μm and has a moisture content of 20 mass% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Powder composition for ceramic molding and method for producing the same

[0001] The present invention relates to a powdered composition for ceramic molding and a method for producing the same, a molded product obtained using the powdered composition for ceramic molding, and a method for producing a ceramic sintered body using the powdered composition for ceramic molding.

[0002] Press molding is a ceramic molding method. In press molding, inorganic particles as ceramic raw materials are generally prepared into granules of several tens of micrometers in size to control fluidity, specific gravity, uniformity, etc. In this process, the granules are prepared by forming a slurry of inorganic particles together with a binder and a dispersant in a solvent such as water, and then spray-drying the slurry (see, for example, Patent Document 1 and Non-Patent Document 1).

[0003] Spray drying requires a large amount of energy. For simple and low-energy production, it is necessary to produce a composition for ceramic molding without granulation by spray drying. However, without granulation, the composition has low fluidity, making it difficult to pack at high density under low pressure during press molding.

[0004] Japanese Patent Application Laid-Open No. 2020-001968

[0005] Yoshihiro Okumoto and three others, "Effect of Dispersion Characteristics of Alumina Slurry on the Structure of Granules and Pressed Compacts," Journal of the Ceramic Society of Japan, 105, [9], p771-774, 1997

[0006] In view of the above, an object of an embodiment of the present invention is to provide a powdery composition for ceramic molding that can be packed at a high density even under low pressure when producing a molded product.

[0007] The present invention includes the following embodiments. [1] A powdery composition for ceramic molding, comprising cellulose nanofibers and inorganic particles having an average particle size of 0.005 μm to 2 μm, and having a moisture content of 20 mass% or less. [2] The powdery composition for ceramic molding according to [1], in which the cellulose nanofiber content is 0.01 mass% to 1.0 mass%. [3] The powdery composition for ceramic molding according to [1] or [2], in which the cellulose nanofibers have anionic functional groups. [4] The powdery composition for ceramic molding according to any one of [1] to [3], in which the cellulose nanofibers have a number-average fiber width of 1 nm to 100 nm. [5] The powdery composition for ceramic molding according to [3] or [4], in which the cellulose nanofibers have an anionic functional group content of 1.0 mmol / g or more. [6] The powdery composition for ceramic molding according to any one of [1] to [5], in which the inorganic particles are primarily composed of at least one selected from the group consisting of metal oxides, silicon compounds, nitrides, and calcium compounds.

[0008] [7] A method for producing the powdery composition for ceramic molding according to any one of [1] to [6], comprising spraying or sprinkling an aqueous dispersion of cellulose nanofibers onto inorganic particles having an average particle size of 0.005 μm or more and 2 μm or less. [8] A molded product obtained by press-molding the powdery composition for ceramic molding according to any one of [1] to [6]. [9] A method for producing a ceramic sintered body, comprising press-molding the powdery composition for ceramic molding according to any one of [1] to [6], and firing the obtained molded product.

[0009] The powdered ceramic molding composition according to the embodiment has excellent fluidity and can be packed at high density even under low pressure during the production of a molded product.

[0010] The powdered composition for ceramic molding according to the embodiment contains cellulose nanofibers and inorganic particles having an average particle size of 0.005 to 2 μm.

[0011] Cellulose nanofibers are fine fibrous cellulose obtained by pulverizing cellulose fibers to the nano level (i.e., less than 1 μm). The number average fiber width of the cellulose nanofibers is preferably 500 nm or less, more preferably 1 to 200 nm, even more preferably 1 to 100 nm, even more preferably 2 to 30 nm, and even more preferably 2 to 10 nm.

[0012] The number average fiber length of the cellulose nanofibers is not particularly limited, and may be, for example, 300 nm to 10 μm, 500 to 5000 nm, 600 to 3000 nm, or 700 to 2000 nm.

[0013] The average aspect ratio of the cellulose nanofibers (number average fiber length / number average fiber width) is not particularly limited, and may be, for example, 10 to 1,000, 20 to 500, or 100 to 300.

[0014] Cellulose nanofibers have a cellulose type I crystal structure. The cellulose type I crystal structure is the crystalline form of natural cellulose, and the cellulose nanofibers are insoluble in water and can maintain their fibrous form in water. The presence of a cellulose type I crystal structure can be identified by the presence of typical peaks at two positions, near 2θ = 14° to 17° and near 2θ = 22° to 23°, in a diffraction profile obtained by wide-angle X-ray diffraction image measurement.

[0015] The cellulose nanofibers may be unmodified and have no anionic functional groups, but preferably have anionic functional groups. By having anionic functional groups, the cellulose nanofibers can be made finer to a higher degree, thereby enabling the molded article to have even higher density and strength.

[0016] Examples of anionic functional groups include at least one selected from the group consisting of a carboxyl group, a phosphate group, a sulfonic acid group, a nitrate group, a boric acid group, and a sulfate group. These anionic functional groups may be directly or indirectly bonded to glucose units, which are structural units of cellulose molecules. When indirectly bonded, an alkylene group having 1 to 4 carbon atoms may be present between the glucose unit and the anionic functional group. One or more anionic functional groups may be bonded to all glucose units constituting the cellulose molecule, or one or more anionic functional groups may be bonded to a portion of the glucose units constituting the cellulose molecule.

[0017] The carboxyl group as the anionic functional group conceptually includes not only the acid form (—COOH) but also the salt form, i.e., the carboxylate group (—COOX, where X is a cation that forms a salt with a carboxylic acid), and the acid form and the salt form may be mixed. Similarly, the phosphate group, sulfonate group, nitrate group, borate group, and sulfate group conceptually include not only the acid form but also the salt form, and the acid form and the salt form may be mixed.

[0018] The salt of the anionic functional group is not particularly limited, and examples thereof include alkali metal salts such as sodium salts and potassium salts, alkaline earth metal salts such as magnesium salts and calcium salts, onium salts such as ammonium salts and phosphonium salts, and amine salts such as primary amines, secondary amines, and tertiary amines. The salt is preferably an alkali metal salt.

[0019] When the cellulose nanofiber has anionic functional groups, the amount of the anionic functional groups (preferably carboxy groups) is not particularly limited, and is preferably, for example, 1.0 mmol / g or more per dry mass of the cellulose nanofiber. The amount of the anionic functional groups is more preferably 1.0 to 3.0 mmol / g, even more preferably 1.2 to 2.8 mmol / g, and even more preferably 1.5 to 2.5 mmol / g.

[0020] The amount of anionic functional groups is measured as follows. For example, in the case of carboxy groups, 60 mL of an aqueous cellulose nanofiber dispersion prepared to a concentration of 0.1 to 1% by mass is adjusted to a pH of approximately 2.5 with a 0.1 mol / L aqueous hydrochloric acid solution, and then a 0.05 mol / L aqueous sodium hydroxide solution is added dropwise to measure the electrical conductivity. This is continued until the pH reaches approximately 11, and the amount of sodium hydroxide (V) consumed in the neutralization stage of the weak acid, where the change in electrical conductivity is gradual, can be used to calculate the amount of anionic functional groups according to the following formula. Phosphate groups can also be measured using similar electrical conductivity measurements. Other anionic functional groups can also be measured using known methods. In this specification, the "dry mass" refers to the mass after drying at 140°C until the rate of mass change per minute is 0.05% or less. Amount of anionic functional groups (mmol / g) = V (mL) × [0.05 / Mass of cellulose nanofiber (g)]

[0021] In one embodiment, the cellulose nanofiber preferably has a carboxy group as the anionic functional group. Examples of cellulose nanofibers containing a carboxy group include oxidized cellulose nanofibers obtained by oxidizing the hydroxyl groups of glucose units in cellulose molecules, and carboxymethylated cellulose nanofibers obtained by carboxymethylating the hydroxyl groups of glucose units in cellulose molecules.

[0022] Oxidized cellulose nanofibers include those in which the hydroxyl group at C6 of the glucose unit in the cellulose molecule has been selectively oxidized to a carboxyl group. Oxidized cellulose nanofibers can be obtained by oxidizing natural cellulose such as wood pulp with a co-oxidant in the presence of an N-oxyl compound, followed by defibration (refining).

[0023] As the N-oxyl compound, a compound having a nitroxy radical, which is generally used as an oxidation catalyst, is used, for example, a piperidine nitroxyoxy radical, with 2,2,6,6-tetramethylpiperidinoxy radical (TEMPO) or 4-acetamido-TEMPO being particularly preferred. Cellulose nanofibers oxidized and refined with TEMPO are generally referred to as TEMPO-oxidized cellulose nanofibers (TOCN). Note that the oxidized cellulose nanofibers may contain aldehyde groups or ketone groups in addition to carboxy groups.

[0024] When cellulose nanofibers are obtained by defibration treatment, the defibration treatment may be carried out after or before the introduction of anionic functional groups. The defibration treatment can be carried out by treating an aqueous dispersion of cellulose fibers using, for example, a homomixer, a high-pressure homogenizer, an ultrasonic dispersion processor, a beater, a disk refiner, a conical refiner, a double-disc refiner, a grinder, or the like under high-speed rotation, to obtain an aqueous dispersion of cellulose nanofibers.

[0025] The inorganic particles blended into the ceramic molding powder composition have an average particle size of 0.005 to 2 μm. By using inorganic particles with such a small average particle size, it is possible to pack the particles densely during the production of a molded product and to suppress the generation of voids during sintering. The average particle size of the inorganic particles is more preferably 0.05 to 1.8 μm, even more preferably 0.1 to 1.5 μm, and even more preferably 0.3 to 1.2 μm.

[0026] Here, the average particle size of the inorganic particles is the average particle size of the inorganic particles in a state in which no cellulose nanofibers are attached. Here, the average particle size of the inorganic particles is the mass-based average diameter (D50) calculated from the particle size distribution measured in a dry state by a laser diffraction / scattering method using a particle size distribution analyzer (MT3000II, Microtrac Bell).

[0027] Examples of inorganic particles include metal oxides, silicon compounds, nitrides, and calcium compounds, and it is preferable that at least one of these is used as the main component. Here, the main component means that the main component accounts for more than 50% by mass, preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, relative to 100% by mass of the total amount of the inorganic particles.

[0028] Examples of the metal oxide include alumina (Al 2 O 3 ), titanium oxide (TiO 2 ), copper oxide (CuO), iron oxide (Fe 2 O 3 ), cobalt oxide (Co 2 O 3 ), zinc oxide (ZnO), zirconia (ZrO 2 ), cerium oxide (CeO 2 ), magnesium oxide (MgO), calcium oxide (CaO), beryllium oxide (BeO), strontium oxide (SrO), barium oxide (BaO), lithium oxide (Li 2 O), sodium oxide (Na 2 O), potassium oxide (K 2 O), yttrium oxide (Y 2 O 3 ), manganese oxide (Mn 2 O 3 ), indium oxide (In 2 O 3 ), tin oxide (SnO 2 ), lanthanum oxide (La 2 O 3 ), praseodymium oxide (Pr 2 O 3 ), neodymium oxide (Nd 2 O 3 ), samarium oxide (Sm 2 O 3 ), europium oxide (Eu 2 O 3 ), gadolinium oxide (Gd 2 O 3 ), terbium oxide (Tb 2 O 3 ), dysprosium oxide (Dy 2O 3 These may be used alone or in combination of two or more.

[0029] Examples of the silicon compound include silicon carbide (SiC) and silicon nitride (Si 3 N 4 These may be used alone or in combination of two or more.

[0030] Examples of the nitride include aluminum nitride (AlN), boron nitride (BN), titanium nitride (TiN), zirconium nitride (ZrN), etc. These may be used alone or in combination of two or more.

[0031] Examples of the calcium compound include lime, calcium phosphate, hydroxyapatite, tricalcium silicate, dicalcium silicate, aluminate, ferrite, calcium sulfate, etc. These may be used alone or in combination of two or more.

[0032] The powdered composition for ceramic molding according to the embodiment contains water in addition to the cellulose nanofibers and inorganic particles, and the moisture content is adjusted to 20% by mass or less. That is, the moisture content is 20% by mass or less relative to the total mass of the composition. Such a low moisture content allows the composition to be in a powder form rather than a slurry form, thereby suppressing aggregation of the inorganic particles. Furthermore, the low moisture content can suppress the generation of voids during sintering, thereby improving the strength of the sintered body. The moisture content of the powdered composition for ceramic molding is preferably 3 to 20% by mass, more preferably 5 to 15% by mass, and even more preferably 7 to 12% by mass.

[0033] In the powdered composition for ceramic molding, the content of cellulose nanofibers is preferably 0.01 to 1.0 mass% relative to the total mass of the composition. Because the amount of cellulose nanofiber added is so small, the generation of voids during sintering can be suppressed, improving the strength of the sintered body. The content of cellulose nanofibers is more preferably 0.01 to 0.5 mass%, even more preferably 0.02 to 0.2 mass%, and even more preferably 0.03 to 0.1 mass%.

[0034] In the powdered composition for ceramic molding, the content of the inorganic particles is not particularly limited, but is preferably 70 to 98 mass % relative to the total mass of the composition, more preferably 75 to 95 mass %, even more preferably 80 to 93 mass %, and even more preferably 82 to 90 mass %.

[0035] The powdered ceramic molding composition may consist only of the above-mentioned cellulose nanofibers, inorganic particles, and water, but may also contain other components, such as binders, dispersants, and lubricants, as long as the effects of the other components are not impaired.

[0036] The powdered composition for ceramic molding according to the embodiment can be produced by spraying or sprinkling an aqueous cellulose nanofiber dispersion onto inorganic particles having an average particle size of 0.005 to 2 μm. That is, the cellulose nanofibers and inorganic particles are mixed by spraying or sprinkling the aqueous cellulose nanofiber dispersion onto the inorganic particles. In this case, the aqueous cellulose nanofiber dispersion may be sprayed or sprinkled onto the inorganic particles while stirring them. This simple process allows the production of a powdered composition for ceramic molding, eliminating the need for spray drying. Therefore, the powdered composition for ceramic molding can be produced easily and with low energy consumption.

[0037] Furthermore, since the powdered composition for ceramic molding according to the embodiment is produced by spraying or sprinkling an aqueous cellulose nanofiber dispersion onto inorganic particles, it is not granulated. That is, the powdered composition for ceramic molding according to the embodiment is a non-granulated powder composition and is distinguished from granulated compositions. Here, granulation refers to solidifying inorganic particles and forming (granulating) them into particles larger than the inorganic particles, and in ceramic press molding applications, spherical particles are generally formed by spray drying.

[0038] The amount of cellulose nanofiber aqueous dispersion used for the above spraying or sprinkling is preferably set so that the moisture content of the powdered composition for ceramic molding falls within the above range, without carrying out a drying step after spraying or sprinkling. That is, it is preferable to spray or sprinkle an amount of cellulose nanofiber aqueous dispersion onto the inorganic particles so that the moisture content of the resulting powdered composition for ceramic molding is 20 mass% or less. Because the inorganic particles are treated to a degree that lightly moistens them with such a small amount of cellulose nanofiber aqueous dispersion, the drying step after the aqueous dispersion treatment can be omitted, further simplifying the process and reducing energy consumption.

[0039] Specifically, the amount of cellulose nanofiber aqueous dispersion to be treated is preferably 3 to 25 parts by mass, more preferably 5 to 20 parts by mass, per 100 parts by mass of inorganic particles.

[0040] The concentration of the cellulose nanofiber aqueous dispersion (the concentration of the cellulose nanofibers as the solid content) is not particularly limited, and can be set so that the content of cellulose nanofibers in the powdered composition for ceramic molding falls within a predetermined range in relation to the treatment amount. The concentration of the cellulose nanofiber aqueous dispersion may be, for example, 0.1 to 5% by mass, or 0.2 to 2% by mass.

[0041] In the powdered ceramic molding composition obtained in this manner, the cellulose nanofibers are adsorbed to the particle surfaces of the inorganic particles. The powdered ceramic molding composition has excellent fluidity due to the effect of the cellulose nanofibers adsorbed to the surfaces of the inorganic particles, allowing for high-density packing even at low pressures. As a result, high-specific-gravity molded products can be molded even at low-pressure press molding. Furthermore, because only a small amount of cellulose nanofiber is added, adverse effects such as the generation of voids during sintering do not occur. These effects make the composition particularly suitable for producing ceramic sintered bodies with complex shapes.

[0042] In the powdered ceramic molding composition obtained by the above-described simple process, the inorganic particles maintain their individual particle size prior to blending, but some particles are loosely aggregated due to the cellulose nanofibers and water adsorbed to the particle surface. Such loosely aggregated particles can be disintegrated by sieving. Therefore, sieving may be performed after spraying or sprinkling. However, it is not necessary to completely disintegrate the individual inorganic particles; some aggregates may be present.

[0043] The sieve to be used after spraying or sprinkling may be, for example, one having a nominal mesh size of 1.4 mm or less, 1 mm or less, or 500 μm or less in accordance with JIS Z8801-1:2019.

[0044] Since cellulose nanofibers are adsorbed onto the particle surfaces of the inorganic particles and some of the inorganic particles are aggregated, the average particle size of the powdered composition for ceramic molding does not necessarily have to be the same as the average particle size of the inorganic particles described above. The average particle size of the powdered composition for ceramic molding is not particularly limited, but is preferably 0.1 to 50 μm, more preferably 0.2 to 30 μm, even more preferably 0.5 to 20 μm, and may be 3 to 15 μm.

[0045] The ceramic molding powder composition can be used for press molding. Press molding can be carried out according to a conventional method, for example, by filling the ceramic molding powder composition into a molding die such as a metal mold or a rubber die and applying pressure. This produces a molded product made of the ceramic molding powder composition.

[0046] The pressure during press molding is not particularly limited, and may be, for example, 5 to 200 MPa, or 10 to 100 MPa. After press molding, cutting may be performed to obtain a molded product of a predetermined shape.

[0047] The obtained molded body is then fired according to a conventional method to obtain a ceramic sintered body. That is, in one embodiment of the method for producing a ceramic sintered body, the above-mentioned powdery composition for ceramic molding is press-molded and the obtained molded body is fired. In addition, the ceramic sintered body according to one embodiment is obtained by firing the above-mentioned molded body. By firing, the inorganic particles are fused and sintered, and the cellulose nanofibers and moisture are removed.

[0048] The temperature at which the molded product is fired is not particularly limited, and may be, for example, 600 to 2000° C. or 800 to 1800° C. After firing, the molded product may be ground and / or polished to form a final product shape.

[0049] Examples will be described in detail below along with comparative examples, but the present invention is not limited to these examples.

[0050] Example 1: 2 g of softwood pulp was mixed with 150 mL of water, 0.25 g of sodium bromide, and 0.025 g of 2,2,6,6-tetramethylpiperidine-1-oxyl (TEMPO). The mixture was thoroughly stirred to disperse the mixture. A 13% by mass aqueous solution of sodium hypochlorite (co-oxidant) was then added to 1.0 g of the pulp, so that the amount of sodium hypochlorite was 6 mmol / g, to initiate the reaction. The temperature was maintained at 20°C during the reaction. As the reaction progressed, the pH decreased, and 0.5 N aqueous solution of sodium hydroxide was added dropwise to maintain the pH at 10-11, while the reaction was continued until no further change in pH was observed (reaction time: 120 minutes). After the reaction was completed, 0.1 N hydrochloric acid was added to adjust the pH to 2 or less, followed by repeated filtration and washing with water for purification. Pure water was added to adjust the solids concentration to 4%.

[0051] The pH of the slurry was then adjusted to 10 with a 24% by mass aqueous solution of sodium hydroxide. The temperature of the slurry was set to 30°C, and sodium borohydride was added in an amount of 0.2 mmol / g relative to the cellulose fibers, followed by a reduction treatment by reacting for 2 hours. After the reaction, 0.1 N hydrochloric acid was added to adjust the pH to 2 or less, and the slurry was purified by repeated filtration and washing with water.

[0052] Pure water was added to the purified cellulose fibers to adjust the final concentration to 0.2% by mass of cellulose fibers. A 24% by mass aqueous solution of sodium hydroxide was added to adjust the pH to 7. This was treated twice at a pressure of 100 MPa using a high-pressure homogenizer (H11, manufactured by Sanwa Engineering) to prepare an aqueous cellulose nanofiber dispersion.

[0053] The cellulose nanofiber aqueous dispersion was sprayed onto alumina (N-92, average particle size 0.5 μm, manufactured by Nishimura Porcelain Co., Ltd.) in an amount of 6 mass % relative to the mass of the alumina while the alumina was being stirred appropriately, and then the mixture was sieved through a sieve with 1.4 mm openings to prepare a powdered composition for ceramic molding. The water content and average particle size of the obtained powdered composition for ceramic molding were measured.

[0054] The ceramic molding powder composition was placed in a mold and press-molded at a pressure of 29.4 MPa to produce a molded product. The molded product was then fired at 1600°C for 16 hours to produce a ceramic sintered body. The density and compressive strength of the resulting ceramic sintered body were measured.

[0055] [Example 2] A powdered ceramic molding composition was prepared in the same manner as in Example 1, except that the concentration of the cellulose nanofiber aqueous dispersion was 0.4 mass %, and the amount of the cellulose nanofiber aqueous dispersion sprayed onto the alumina was 12 mass % relative to the mass of the alumina. The moisture content and average particle size were measured, and molded products and sintered ceramic bodies were produced, and the density and compressive strength were measured.

[0056] [Example 3] A powdered ceramic molding composition was prepared in the same manner as in Example 1, except that the concentration of the cellulose nanofiber aqueous dispersion was 1.0 mass %, and the amount of the cellulose nanofiber aqueous dispersion sprayed onto the alumina was 25 mass % relative to the mass of the alumina. The moisture content and average particle size were measured, and molded products and sintered ceramic bodies were produced, and the density and compressive strength were measured.

[0057] [Examples 4 and 5] In Example 4, titanium oxide (3YI-R, manufactured by Toray Industries, Inc., average particle size 0.5 μm) was used instead of alumina. In Example 5, silicon nitride (SN2400, manufactured by Kyocera Corporation, average particle size 1.0 μm) was used instead of alumina. Except for these, in the same manner as in Example 2, a powdery composition for ceramic molding was prepared, and measurements of the water content and average particle size, molded products and sintered ceramic bodies were produced, and measurements of density and compressive strength were carried out.

[0058] [Example 6] A powdered composition for ceramic molding was prepared in the same manner as in Example 2, except that the high-pressure homogenizer treatment conditions during the preparation of the cellulose nanofiber aqueous dispersion were changed to a single treatment at a pressure of 50 MPa. The moisture content and average particle size were measured, and molded products and ceramic sintered bodies were produced, and the density and compressive strength were measured.

[0059] [Example 7] A powdered composition for ceramic molding was prepared in the same manner as in Example 2, except that the amount of sodium hypochlorite added during the preparation of the cellulose nanofiber aqueous dispersion was 3 mmol / g. The moisture content and average particle size were measured, and molded products and ceramic sintered bodies were produced, and the density and compressive strength were measured.

[0060] Example 8 A powdered ceramic molding composition was prepared in the same manner as in Example 2, except that WFo-1002 (mechanically defibrated cellulose nanofiber, manufactured by Sugino Machine Co., Ltd.) was used as the cellulose nanofiber aqueous dispersion and its concentration was set to 0.2 mass %, and measurements of the water content and average particle size, production of molded products and ceramic sintered bodies, and measurements of density and compressive strength were carried out.

[0061] Comparative Example 1 A powdered ceramic molding composition was prepared in the same manner as in Example 2, except that the amount of cellulose nanofiber aqueous dispersion sprayed onto the alumina was 30 mass % relative to the mass of the alumina. The moisture content and average particle size were measured, a molded product and a ceramic sintered body were produced, and the density and compressive strength were measured.

[0062] Comparative Example 2 A powdered ceramic molding composition was prepared in the same manner as in Example 2, except that a 0.2 mass% aqueous solution of sodium polycarboxylate was used instead of the aqueous cellulose nanofiber dispersion. The moisture content and average particle size were measured, a molded product and a sintered ceramic body were produced, and the density and compressive strength were measured.

[0063] The measurement methods are as follows, and the results are shown in Table 1. In Table 1, "CNF" means cellulose nanofiber.

[0064] [Measurement of number average fiber width, number average fiber length, and average aspect ratio] The number average fiber width and number average fiber length of the cellulose nanofibers were observed using an atomic force microscope (AFM, manufactured by Hitachi High-Tech Corporation). Specifically, each cellulose nanofiber aqueous dispersion was cast onto a mica substrate, and 10 AFM images were taken. 25 cellulose nanofibers were selected from the images, and the fiber width and fiber length were measured. From the obtained fiber width and fiber length data, the arithmetic means were calculated to determine the number average fiber width [nm] and number average fiber length [nm]. The average aspect ratio was also calculated according to the following formula: Average aspect ratio = Number average fiber length [nm] / Number average fiber width [nm]

[0065] [Measurement of Carboxy Group Amount] 60 mL of an aqueous cellulose nanofiber dispersion prepared to a concentration of 0.1% by mass was adjusted to a pH of approximately 2.5 with a 0.1 mol / L aqueous hydrochloric acid solution, and then a 0.05 mol / L aqueous sodium hydroxide solution was added dropwise to measure the electrical conductivity. Measurements were continued until the pH reached approximately 11, and the amount of carboxy groups was calculated from the amount of sodium hydroxide V [mL] consumed in the neutralization stage of the weak acid, where the change in electrical conductivity is gradual, according to the following formula: Amount of Carboxy Groups (mmol / g) = V (mL) × [0.05 / Mass of Cellulose Nanofiber (g)]

[0066] [Measurement of Moisture Content] The moisture content of the powdered ceramic molding composition was measured using an infrared heating moisture meter (MX-50 manufactured by A&D, 120° C., 60 minutes).

[0067] [Measurement of average particle size of powder composition] The average particle size of the powder composition for ceramic molding was measured in a dry state by a laser diffraction / scattering method using a particle size distribution analyzer (MT3000II, Microtrac Bell Co., Ltd.) The mass-based average diameter (D50) calculated from the particle size distribution was taken as the average particle size.

[0068] [Measurement of Density] The bulk density of the ceramic sintered body was measured in accordance with JIS R 1634:1998.

[0069] [Measurement of Compressive Strength] The compressive strength of the ceramic sintered body was measured in accordance with JIS R 1608:2003.

[0070]

[0071] As shown in Table 1, the powdered ceramic molding compositions according to Examples 1 to 8 were packed at high density even though the press molding was carried out at a low pressure, and therefore the ceramic sintered bodies produced using these compositions had high density and high strength.

[0072] In contrast, in Comparative Example 1, in which the ceramic molding powder composition had a high moisture content, the moisture caused voids in the ceramic sintered body, resulting in a low density and low compressive strength of the ceramic sintered body.

[0073] Furthermore, in Comparative Example 2, in which sodium polycarboxylate was used instead of cellulose nanofibers, the powdered ceramic molding composition had low fluidity, and therefore was not packed densely when pressed at low pressure, and cracks occurred during compression by press molding, making it impossible to perform firing or subsequent evaluation.

[0074] The various numerical ranges described in this specification can be arbitrarily combined with their respective upper and lower limit values, and all such combinations are considered to be preferred numerical ranges described in this specification. Furthermore, a numerical range described as "X to Y" means from X to Y.

[0075] Although several embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their omissions, substitutions, modifications, etc. are included within the scope and spirit of the invention, as well as within the scope of the invention described in the claims and their equivalents.

Claims

1. A powdered composition for ceramic molding, comprising cellulose nanofibers and inorganic particles having an average particle size of 0.005 μm or more and 2 μm or less, and having a moisture content of 20 mass% or less.

2. The powdered composition for ceramic molding according to claim 1, wherein the content of the cellulose nanofibers is 0.01% by mass or more and 1.0% by mass or less.

3. The powdered ceramic molding composition according to claim 1, wherein the cellulose nanofibers have anionic functional groups.

4. The powdery composition for ceramic molding according to claim 1, wherein the number average fiber width of the cellulose nanofibers is 1 nm or more and 100 nm or less.

5. The powdery composition for ceramic molding according to claim 3, wherein the amount of anionic functional groups in the cellulose nanofibers is 1.0 mmol / g or more.

6. The powdered ceramic molding composition according to claim 1, wherein the inorganic particles are primarily composed of at least one selected from the group consisting of metal oxides, silicon compounds, nitrides, and calcium compounds.

7. A method for producing a powdered composition for ceramic molding according to any one of claims 1 to 6, comprising spraying or sprinkling an aqueous dispersion of cellulose nanofibers onto inorganic particles having an average particle size of 0.005 μm or more and 2 μm or less.

8. A molded product obtained by press-molding the powder composition for ceramic molding according to any one of claims 1 to 6.

9. A method for producing a ceramic sintered body, comprising press-molding the powder composition for ceramic molding according to any one of claims 1 to 6, and firing the resulting molded body.

Citation Information

Patent Citations

  • Manufacture of ceramic honeycomb structure

    JP1989195006A

  • Alumina substrate for mounting photoelectric conversion element and its manufacturing method

    JP2006062912A

  • Binder for wet molding

    JP2018065727A

  • Extrusion molding composition, and method for producing extrusion molding

    JP2019131427A

  • Ceramic binder

    JP2019151690A