Coil spring manufacturing method
The method of alternating current heating and subsequent shot peening in coil spring manufacturing addresses the challenge of balancing residual stress and hardness, resulting in improved fatigue and corrosion resistance by selectively reducing tensile residual stress and controlling hardness distribution.
Patent Information
- Application Number
- PCT/JP2024/011924
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-03
AI Technical Summary
Existing methods for manufacturing coil springs fail to achieve a suitable balance between residual stress and hardness, as high heating temperatures can reduce hardness while insufficient heating may not adequately reduce tensile residual stress.
A method involving alternating current heating, where the inner diameter side of the wire is heated to a higher temperature than the outer diameter side, followed by shot peening to apply compressive residual stress, effectively reducing tensile residual stress and controlling hardness distribution.
This approach allows for the achievement of suitable residual stress and hardness in coil springs, enhancing fatigue resistance and corrosion fatigue resistance while minimizing the risk of early breakage.
Smart Images

Figure JP2024011924_03102024_PF_FP_ABST
Abstract
Description
Coil spring manufacturing method
[0001] The present invention relates to a method for manufacturing a coil spring.
[0002] When manufacturing a coil spring, the wire is subjected to various heat treatments such as quenching, tempering, and annealing. As a method for heating the wire in the heat treatment, induction heating using a high-frequency heating coil is known, as described in, for example, Patent Document 1. Other heating methods include, for example, direct current heating, in which a direct current is passed through the wire to generate heat.
[0003] Patent No. 6053916
[0004] Annealing reduces the residual tensile stress that occurs in the wire during coiling. The effect of reducing the residual tensile stress increases as the heating temperature increases. However, if the heating temperature is too high, the overall hardness of the wire may decrease.
[0005] As described above, there is still room for improvement in the heat treatment of the wire of a coil spring. Therefore, one object of the present invention is to provide a method for manufacturing a coil spring that can achieve suitable residual stress and hardness.
[0006] A method for manufacturing a coil spring according to one embodiment includes forming a wire into a spiral shape, attaching first and second terminals to the wire, the first and second terminals being connected to a power source capable of supplying alternating current, and passing an alternating current through the wire through the first and second terminals to heat the wire with a temperature distribution in which the temperature of an inner diameter side portion of the wire is higher than the temperature of an outer diameter side portion. After the forming and before the heating, the wire has a higher tensile residual stress in the inner diameter side portion than in the outer diameter side portion. The heating reduces the tensile residual stress in the inner diameter side portion and reduces the hardness of the inner diameter side portion below the hardness of the outer diameter side portion.
[0007] Compressive residual stress may be imparted to the inner diameter side portion and the outer diameter side portion by shot peening the wire after the heating.
[0008] For example, in the temperature distribution, it is preferable that the temperature of the axis of the wire is lower than the temperatures of the inner diameter side portion and the outer diameter side portion.
[0009] An electrically floating conductor may be disposed inside the strand formed into a spiral shape, and the heating may be performed with the conductor disposed therein.
[0010] Furthermore, a ferromagnetic material may be disposed on the outside of the wire formed into a spiral shape, and the heating may be performed with the ferromagnetic material disposed.
[0011] According to the present invention, it is possible to provide a method for manufacturing a coil spring that can achieve suitable residual stress and hardness.
[0012] FIG. 1 is a schematic perspective view of a coil spring according to a first embodiment. FIG. 2 is a schematic cross-sectional view showing an example of a structure that can be applied to a coil spring. FIG. 3 is a graph showing an example of residual stress distribution of a wire in an effective portion. FIG. 4 is a graph showing an example of hardness distribution of a wire in an effective portion. FIG. 5 is a flowchart showing an example of a manufacturing process of a coil spring. FIG. 6 is a diagram showing a schematic configuration of an AC current heating device that can be used for annealing. FIG. 7 is a graph showing an example of residual stress distribution of a wire in a manufacturing process of a coil spring. FIG. 8 is a graph showing an example of temperature distribution of a wire during annealing. FIG. 9 is a graph showing experimental results of annealing using AC current heating. FIG. 10 is a graph showing the relationship between residual stress after annealing, heating time, and heating temperature in annealing. FIG. 11 is a diagram showing a first modified example of an AC current heating device. FIG. 12 is a schematic diagram for explaining the proximity effect. FIG. 13 is a diagram showing a second modified example of an AC current heating device. FIG. 14 is a schematic cross-sectional view of a coil spring according to a second embodiment. Fig. 15 is a graph showing the temperature distribution during annealing according to a comparative example. Fig. 16 is a graph showing an example of the residual stress distribution of a wire before and after annealing. Fig. 17 is a graph showing an example of the hardness distribution of a wire before and after annealing according to a comparative example. Fig. 18 is a graph showing an example of the hardness distribution of a wire before and after annealing according to the present embodiment.
[0013] Several embodiments will be described with reference to the drawings. The use of the coil spring disclosed in each embodiment is not particularly limited, but as an example, it can be used in a suspension system for a vehicle.
[0014] 1 is a schematic perspective view of a coil spring 1 according to a first embodiment. The coil spring 1 has a wire 2 wound in a spiral shape around a coil axis X1. For example, the wire 2 is formed from spring steel, and its surface 20 is entirely covered with a coating 21. In the following description, an axial direction DX parallel to the coil axis X1 and a radial direction DR centered on the coil axis X1 are defined.
[0015] The coil spring 1 has an effective portion 10, a first end winding portion 11, and a second end winding portion 12. The effective portion 10 is located between the first end winding portion 11 and the second end winding portion 12. For example, the first end winding portion 11 is in a range of approximately one turn from the first terminal 2a of the wire 2, and the second end winding portion 12 is in a range of approximately one turn from the second terminal 2b of the wire 2. The wire 2 is wound multiple times in the effective portion 10.
[0016] 2 is a schematic cross-sectional view showing an example of a structure that can be applied to the coil spring 1. This cross-section corresponds to a transverse cross-section perpendicular to the axis X2 of the wire 2. As shown in the figure, a circumferential direction Dθ is defined with the axis X2 as the center.
[0017] In the following description, of the two intersections where the center line CL, which is perpendicular to the coil axis X1 and passes through the axis X2 of the wire 2, intersects with the surface 20, the intersection on the coil axis X1 side (inner diameter side) will be referred to as position Q1, and the intersection on the opposite side from the coil axis X1 (outer diameter side) will be referred to as position Q2. Furthermore, the portion of the wire 2 that is closer to the coil axis X1 than the axis X2 in the radial direction DR (the left half of the wire 2 shown in FIG. 2) will be referred to as the inner diameter side portion IP, and the portion of the wire 2 that is farther from the coil axis X1 than the axis X2 in the radial direction DR (the right half of the wire 2 shown in FIG. 2) will be referred to as the outer diameter side portion OP.
[0018] The wire 2 has a first layer L1 and a second layer L2 (the portion with a dotted pattern) that is softer than the first layer L1. The first layer L1 covers most of the cross section of the wire 2 and includes the axis X2. The second layer L2 is formed in a region of the surface 20 on the inner diameter side and inside the wire 2 near that region.
[0019] 2, the first layer L1 includes the position Q2, and the second layer L2 includes the position Q1. The outer diameter side portion OP is entirely made up of the first layer L1, and the inner diameter side portion IP is made up of the first layer L1 and the second layer L2. On the surface 20 of the wire 2 configured in this manner, a soft region (the second layer L2) and a hard region (the first layer L1) are aligned in the circumferential direction Dθ.
[0020] The range in which the second layer L2 is provided is not limited to the example shown in Fig. 2. For example, the second layer L2 may be provided in a narrower or wider range than that shown in Fig. 2. The second layer L2 may extend to the outer diameter side portion OP. Furthermore, the wire 2 may further include another layer having a hardness different from that of the first layer L1 and the second layer L2.
[0021] The wire 2 may have the cross-sectional structure shown in Fig. 2 throughout the entire wire between the first terminal 2a and the second terminal 2b. As another example, the hardness distribution in the cross section may be different in the active portion 10, the first end winding portion 11, and the second end winding portion 12.
[0022] 3 is a graph showing an example of the residual stress distribution σ of the wire 2 in the effective portion 10. In this graph, the vertical axis represents the residual stress, and the horizontal axis represents the position inside the wire 2 along the center line CL shown in FIG. 2. The positive (+) region on the vertical axis represents tensile residual stress, and the negative (-) region represents compressive residual stress. Note that the residual stress in this embodiment refers to the stress in a direction tilted 45 degrees from the axis X2 (the principal stress direction of the coil spring 1).
[0023] By subjecting the spirally wound wire 2 to shot peening, which will be described later, compressive residual stress is imparted near positions Q1 and Q2. In the example of FIG. 3, tensile residual stress is imparted near axis X2. Furthermore, the peak of the compressive residual stress in the inner diameter side portion IP and the peak of the compressive residual stress in the outer diameter side portion OP are equivalent. However, these peaks may be different. As an example, these peaks are located approximately 0.1 mm (0.05 to 0.2 mm) from the surface 20.
[0024] 4 is a graph showing an example of the hardness distribution H of the wire 2 in the effective portion 10. In this graph, the vertical axis represents hardness (e.g., Vickers hardness HV), and the horizontal axis represents the position inside the wire 2 along the center line CL shown in FIG.
[0025] In the example of Figure 4, the hardness of the first layer L1 is constant. On the other hand, the hardness of the second layer L2 gradually decreases from the axis X2 side toward position Q1. The width of the second layer L2 along the center line CL is sufficiently smaller than the width of the first layer L1 along the center line CL. In other words, the second layer L2 is formed on the surface layer of the wire 2. As an example, the width of the second layer L2 along the center line CL (depth from position Q1) is 20% or less of the wire diameter of the wire 2.
[0026] The hardness distribution H of the wire 2 is not limited to the example shown in FIG. 4 . For example, the second layer L2 may have a V-shaped decreasing hardness distribution. Furthermore, the hardness near the position Q2 may be lower than the hardness near the axis X2. In this case, the hardness near the position Q1 may be even lower than the hardness near the position Q2.
[0027] The residual stress distribution and hardness distribution in the effective portion 10 may be constant over the entire length or may vary partially. The residual stress distribution and hardness distribution in the end turn portions 11, 12 may be the same as or different from those in the effective portion 10. In one example, a larger compressive residual stress is imparted to the outer diameter side portions OP of the end turn portions 11, 12 than to the outer diameter side portion OP of the effective portion 10.
[0028] Next, a method for manufacturing the coil spring 1 will be described. Fig. 5 is a flowchart showing an example of the manufacturing process for the coil spring 1. This example corresponds to so-called cold forming, in which the wire 2 is first quenched before being coiled (step P1). The wire 2 is then tempered (step P2). For example, induction heating can be used for these quenching and tempering processes.
[0029] After tempering, the cooled wire 2 is formed into a spiral shape using a coiling machine (process P3). After process P3, the spirally formed wire 2 is annealed (process P4). Furthermore, the wire 2 is subjected to shot peening (process P5). This shot peening imparts compressive residual stress to the wire 2. Thereafter, the coil spring 1 is completed through processes such as setting and forming a coating film 21.
[0030] Immediately after the coiling in step P3, the wire 2 is entirely formed of the first layer L1. By the subsequent annealing in step P4, the wire 2 is partially softened and the second layer L2 is formed.
[0031] The manufacturing process of the coil spring 1 is not limited to that shown in Fig. 5. For example, after the annealing in step P4, a softening treatment may be performed to reduce the hardness of the entire or part of the wire 2 near the surface 20. The softening treatment may be performed on specific portions, such as the end turn portions 11 and 12. The softening treatment may also be performed at other times, such as before the coiling in step P3.
[0032] 6 is a diagram showing a schematic configuration of an AC current heating device 100 (hereinafter referred to as heating device 100) that can be used in the annealing of process P4. The heating device 100 includes a first terminal 3A, a second terminal 3B, and a control device 4.
[0033] The control device 4 includes a power supply 41 that supplies AC current. The first terminal 3A and the second terminal 3B are connected to the power supply 41 via wiring. The frequency of the AC current supplied by the power supply 41 is not particularly limited, but as an example, a high frequency of 1 kHz or higher may be used.
[0034] 6, each of the first terminal 3A and the second terminal 3B is divided into a first portion 31 and a second portion 32. The first terminal 3A and the second terminal 3B can be attached to the wire 2 by sandwiching a part of the wire 2 between the first portion 31 and the second portion 32. However, the structure for attaching the first terminal 3A and the second terminal 3B to the wire 2 is not limited to this example.
[0035] When performing a heating treatment using the heating device 100, a first terminal 3A and a second terminal 3B are attached to the spirally formed wire 2. In the example of Fig. 6, the first portion 31 and the second portion 32 of the first terminal 3A clamp the vicinity of the first terminal 2a of the wire 2. Also, the first portion 31 and the second portion 32 of the second terminal 3B clamp the vicinity of the second terminal 2b of the wire 2.
[0036] When the first terminal 3A and the second terminal 3B are attached to the wire 2, a circuit is formed in which these elements are connected in series with the power source 41. The control device 4 starts to energize the wire 2 in response to an operator's switch operation or an external control signal. In Figure 6, solid arrows indicate an example of the direction of current flow. This direction switches periodically depending on the frequency of the power source 41.
[0037] This current application heats at least a portion of the wire 2. The frequency, amplitude, and current application time of the AC current can be determined appropriately depending on the shape of the wire 2 (e.g., wire diameter, cross-sectional shape, coil diameter, pitch, number of turns, coil length, material), the part to be heated, the target heating temperature, etc. When it is time to stop heating, the control device 4 stops the current supply from the power source 41.
[0038] Thereafter, the wires 2 are cooled. This cooling may be natural cooling, or, if rapid cooling is required, may be performed by spraying a fluid such as water or air onto the wires 2.
[0039] When an AC current flows through the wire 2, the skin effect increases the current density near the surface 20. Furthermore, in the wire 2 formed into a spiral shape, the current path passing through the inner diameter side region of the surface 20 is short, so the current density near the inner diameter side region is likely to increase.
[0040] By utilizing these, it is possible to intensively heat a portion of the inner diameter side portion IP close to the surface 20, and form the second layer L2 in the heated portion as shown in Fig. 2. The range of the second layer L2 and the depth of the second layer L2 from the surface 20 can be adjusted by, for example, the current application time (heating time) and the frequency of the AC current.
[0041] In order to maintain the hardness of the inside of the wire 2, it is preferable to carry out the above-mentioned cooling after the heating is completed and before the temperature inside rises due to heat transfer from the vicinity of the heated surface 20.
[0042] 7 is a graph showing an example of the residual stress distribution of the wire 2 in the manufacturing process of the coil spring 1. The residual stress distribution shown in this graph indicates the residual stress in the effective portion 10, similar to, for example, FIG.
[0043] Residual stress distribution σ1 indicates the residual stress in the wire 2 immediately after coiling in process P3 (before annealing in process P4). Residual stress distribution σ2 indicates the residual stress in the wire 2 immediately after annealing in process P4 (before shot peening in process P5). Residual stress distribution σ3 indicates the residual stress after shot peening in process P5, and is similar to the residual stress distribution σ shown in FIG. 3.
[0044] As can be seen from the residual stress distribution σ1, tensile residual stress occurs in the inner diameter side portion IP immediately after process P3. This tensile residual stress becomes larger, for example, toward the surface layer of the wire 2. On the other hand, almost no residual stress occurs in the outer diameter side portion OP. However, tensile residual stress or compressive residual stress having an absolute value smaller than that of the tensile residual stress in the inner diameter side portion IP may occur in the outer diameter side portion OP.
[0045] 8 is a graph showing an example of a temperature distribution T of the wire 2 during annealing in process P4. In this graph, the vertical axis represents temperature [°C], and the horizontal axis represents the position inside the wire 2 along the center line CL shown in FIG.
[0046] When an AC current is applied to the wire 2 using the heating device 100 shown in Figure 6, the temperature near the surface 20 rises due to the skin effect. Furthermore, the temperature of the inner diameter side portion IP, which has a shorter current path, rises compared to the temperature of the outer diameter side portion OP. As a result, the temperature at position Q1 is higher than the temperature at position Q2, and the temperature near the axis X2 is lower than the temperatures at positions Q1 and Q2. The temperature at position Q1 is, for example, 400°C or higher, and in Figure 8, it is 500°C or higher.
[0047] When annealing is performed with such a temperature distribution T, the inner diameter side portion IP is heated preferentially. Therefore, the tensile residual stress in the inner diameter side portion IP is reduced, as shown by the residual stress distribution σ2 in FIG. 7. Note that the tensile residual stress in the inner diameter side portion IP does not necessarily need to be completely eliminated, but only needs to be reduced compared to the residual stress distribution σ1. When residual stress occurs in the outer diameter side portion OP in the residual stress distribution σ1, the residual stress may be reduced by annealing.
[0048] When the shot peening in process P5 is performed, compressive residual stress is imparted near the surface 20 of the wire 2, as shown by the residual stress distribution σ3. During shot peening, the shot material is more likely to strike the outer diameter side region of the surface 20, but less likely to strike the inner diameter side region of the surface 20. In this case, it is possible that compressive residual stress is imparted to a deep position in the outer diameter side portion OP, while compressive residual stress is imparted only to a shallow position in the inner diameter side portion IP. In this case, the peak of the compressive residual stress in the outer diameter side portion OP shown in FIG. 7 may be greater than the peak of the compressive residual stress in the inner diameter side portion IP.
[0049] During annealing, the hardness of the portion of the wire 2 that is heated to a high temperature decreases. That is, when the wire 2 is heated according to the temperature distribution T in Fig. 8, the hardness of the inner diameter side portion IP, particularly near the surface 20, decreases (softens), and the hardness distribution H shown in Fig. 4 is obtained.
[0050] Note that the hardness of at least a portion of the outer diameter side portion OP near the surface 20 may be reduced. In this case, based on the temperature distribution T in Fig. 8 , the degree of reduction in hardness of the outer diameter side portion OP is smaller than the degree of reduction in hardness of the inner diameter side portion IP. In other words, the inner diameter side portion IP is preferentially softened.
[0051] Generally, to ensure the sag resistance of a coil spring, it is necessary to increase the hardness of the wire. However, if the wire is too hard, corrosion pits that occur near the surface will cause cracks to grow more quickly, increasing the risk of early breakage of the coil spring. In addition, stress is more likely to be applied to the inner diameter area of the wire surface, making it more susceptible to corrosion fatigue.
[0052] In contrast, in this embodiment, the wire 2 has a hard first layer L1 and a soft second layer L2. Furthermore, the first layer L1 covers most of the cross section of the wire 2, including the axis X2 and the outer diameter side portion OP, and the second layer L2 is located near the surface 20 of the inner diameter side portion IP. With this configuration, the first layer L1 ensures good sag resistance of the coil spring 1. In addition, the second layer L2 reduces the risk of breakage and improves the corrosion fatigue resistance of the coil spring 1.
[0053] Here, for example, assume that direct current heating is used for the annealing in step P4 instead of alternating current heating. When direct current is passed through the wire 2, the skin effect described above does not occur, and the heating temperature distribution in the cross section of the wire 2 is relatively uniform. In this case, the wire 2 is heated to a high temperature up to the vicinity of the axis X2, and if the temperature is too high, the wire 2 will soften overall. On the other hand, if the heating temperature is lowered to maintain good hardness after annealing, the residual stress caused by coiling cannot be sufficiently reduced. Similar problems to those described here can occur when annealing the wire 2 using a heating furnace or induction heating.
[0054] In contrast, in this embodiment, by using AC current heating, it is possible to perform annealing in a temperature distribution T in which the inner diameter side portion IP is at a high temperature, as shown in Fig. 8. This makes it possible to effectively reduce the tensile residual stress in the inner diameter side portion IP and to suppress a decrease in hardness in the vicinity of the axis X2 and in the outer diameter side portion OP.
[0055] For example, the hardness at position Q1 after annealing is preferably reduced by 10% or more, more preferably by 15% or more, compared to the hardness before annealing. In one example, the hardness before annealing is 600 HV and the hardness after annealing is 500 HV.
[0056] The inventors conducted an experiment to verify the effect of removing residual stress by annealing using AC current heating. In this experiment, AC current heating was applied to a coil spring having a wire diameter of 8.8 mm, and the residual stress distribution was measured under multiple heating conditions.
[0057] 9 is a graph showing the experimental results. The vertical axis represents residual stress [MPa], and the horizontal axis represents the distance [mm] from the inner diameter surface of the wire. The heating conditions for the wire were as follows: [440°C x 1 second] The inner diameter surface was heated to 440°C in 1 second by passing an AC current, and then the current was stopped. [440°C x 2 seconds] The inner diameter surface was heated to 440°C in 2 seconds by passing an AC current, and then the current was stopped. [440°C x 4 seconds] The inner diameter surface was heated to 440°C in 4 seconds by passing an AC current, and then the current was stopped. [400°C x 4 seconds] The inner diameter surface was heated to 400°C in 4 seconds by passing an AC current, and then the current was stopped.
[0058] 10 is a graph showing the relationship between the residual stress after annealing and the heating time and heating temperature during annealing. The plots in this graph show the residual stress after annealing at a position 0.2 mm from the inner diameter surface for annealing at a heating temperature of 440°C, annealing at a heating temperature of 400°C, and before annealing.
[0059] As can be seen from the graph in Figure 9, under all heating conditions, the residual stress near the inner diameter surface (for example, in the range of 0 mm to 0.5 mm) is reduced compared to before annealing. Furthermore, as can be seen from the graph in Figure 10, the longer the heating time, the more the residual stress is reduced. Furthermore, for the same heating time, the higher the heating temperature, the more the residual stress is reduced.
[0060] Based on the above experiments, it was shown that annealing by AC current heating can reduce the tensile residual stress near the inner diameter surface. Furthermore, it was also shown that the effect of reducing the tensile residual stress can be appropriately adjusted by the heating temperature and time.
[0061] The matter disclosed in this embodiment can be modified in various ways. For example, the configuration of the heating device 100 for performing AC heating is not limited to that shown in FIG.
[0062] 11 is a diagram showing a first modified example of the heating device 100. This heating device 100 differs from the heating device 100 in that it further includes a conductor 5 in addition to the elements shown in FIG.
[0063] The conductor 5 has, for example, a cylindrical or columnar shape and is made of a metal material with excellent conductivity such as copper, aluminum, etc. The conductor 5 may also have a laminated structure of a conductive layer made of a metal material and an insulating layer made of a resin or the like.
[0064] When annealing is performed using such a heating device 100, a first terminal 3A and a second terminal 3B are attached to the spirally wound wire 2. Furthermore, a conductor 5 is placed inside the wire 2. At this time, the conductor 5 is in an electrically floating state and is insulated from other conductive elements such as the wire 2. The conductor 5 is supported, for example, by an insulating member (not shown).
[0065] Here, the role of the conductor 5 will be explained. When a current flows through a workpiece such as the wire 2, if an electrically floating conductor is placed nearby, a so-called proximity effect occurs. In the heating device 100 shown in Fig. 11, this proximity effect is utilized to control the current density distribution (heating temperature distribution) of the wire 2. In other words, the conductor 5 is placed at a position where the proximity effect occurs in the wire 2.
[0066] 12 is a schematic diagram for explaining the proximity effect, showing a rod-shaped workpiece Ws and a conductor 5s arranged in the vicinity thereof. A current I from a power source flows into the workpiece Ws. A When the magnetic field H flows, a magnetic field H IA occurs (Ampere's law).
[0067] In the conductor 5s, this magnetic field H IA The eddy current I caused by E1 is generated (Lenz's law). Furthermore, the eddy current I E1 The magnetic field H caused by IE is generated around the conductor 5s. This magnetic field H IE acts on the workpiece Ws, an eddy current I E2 occurs.
[0068] current I A , eddy current I E1 and eddy current I E2 The direction of the current I flows is as shown by the arrow in the figure. That is, in the workpiece Ws, the current I flows in the vicinity of the side surface far from the conductor 5s.A The direction of the eddy current I E2 On the other hand, in the vicinity of the side surface closer to the conductor 5s, the current I A The direction of the eddy current I E2 As a result, the current density of the workpiece Ws becomes higher near the side surface closer to the conductor 5s.
[0069] By utilizing this proximity effect, it is possible to control the current density distribution and heating temperature distribution of the workpiece Ws. That is, when the conductor 5 is placed inside the wire 2 as shown in Figure 11, the current density near the surface on the inner diameter side of the wire 2 increases, and the heating temperature near the surface also increases. This makes it possible to heat the inner diameter side more intensively than when the conductor 5 is not used.
[0070] 13 is a diagram showing a second modified example of the heating device 100. In the example shown in this figure, the heating device 100 further includes a ferromagnetic body 6 in addition to the conductor 5. The ferromagnetic body 6 can be made of, for example, ferrite, but is not limited to this example.
[0071] The ferromagnetic body 6 is, for example, cylindrical and is arranged to surround the wire 2. The ferromagnetic body 6 has a function of influencing the magnetic flux generated when a current is passed through the wire 2, and inducing the current density toward the inner diameter side of the wire 2. By using the magnetic flux induction function of the ferromagnetic body 6 in addition to the proximity effect of the conductor 5, the heating temperature of the wire 2 can be controlled with greater precision.
[0072] In addition to the first and second modified examples described above, various configurations may be adopted for the heating device 100 used in annealing. For example, the heating device 100 may include the ferromagnetic body 6 without including the conductor 5.
[0073] [Second embodiment] Fig. 14 is a schematic cross-sectional view of a coil spring 1 according to a second embodiment. In the coil spring 1 according to this embodiment, the hardness of the inside of the wire 2 is higher than that of the vicinity of the surface 20. That is, like the first embodiment, the wire 2 has a first layer L1 including the axis X2 and a second layer L2 having a lower hardness than the first layer L1, but in the example of Fig. 14, the second layer L2 surrounds the entire periphery of the first layer L1.
[0074] A coil spring 1 having such a configuration can be manufactured by using a wire 2 whose internal hardness has been increased before coiling, for example. In other words, the second layer L2 of the coil spring 1 according to this embodiment is not caused only by heating the wire 2 according to the temperature distribution T in FIG. 8 during annealing as in the first embodiment, but is formed on the wire 2 mainly before annealing.
[0075] The same method as in the first embodiment can be applied to the manufacturing method of the coil spring 1 according to this embodiment. An example of the effect in this case will be described below with reference to Figs.
[0076] 15 is a graph showing temperature distributions during annealing in a comparative example compared to this embodiment. Both temperature distributions Ta and Tb shown in this figure are uniform within the cross section of the wire 2. Temperature distribution Ta is a temperature that can sufficiently remove the tensile residual stress of the wire 2, and temperature distribution Tb is a temperature lower than temperature distribution Ta. In one example, temperature distribution Ta is 500°C, and temperature distribution Tb is 400°C.
[0077] 16 is a graph showing an example of residual stress distribution in the wire 2 before and after annealing. In the graph, residual stress distribution σ1 indicates the residual stress in the wire 2 immediately after coiling (before annealing). Residual stress distributions σ2a and σ2b indicate the residual stress in the wire 2 immediately after annealing (before shot peening) using temperature distributions Ta and Tb, respectively.
[0078] 17 and 18 are graphs showing an example of the hardness distribution of the wire 2 before and after annealing. The graph in Fig. 17 corresponds to a comparative example in which annealing is performed using the temperature distributions Ta and Tb shown in Fig. 15. The graph in Fig. 18 corresponds to a case in which annealing is performed using the temperature distribution T in Fig. 8 obtained by AC current heating described in the first embodiment. In each of Figs. 17 and 18, hardness distribution H1 indicates the hardness distribution of the wire 2 before annealing. Furthermore, hardness distributions H2a, H2b, H2c, and H2d indicate the hardness distribution of the wire 2 after annealing.
[0079] In the residual stress distribution σ1 shown in Figure 16, tensile residual stress occurs in the inner diameter side portion IP, as in Figure 7. The temperature distribution Ta in Figure 15 is a temperature high enough to eliminate this tensile residual stress. Therefore, when annealing is performed at the temperature distribution Ta, the tensile residual stress in the inner diameter side portion IP is eliminated, as shown in the residual stress distribution σ2a. However, when annealing is performed at such a high temperature, the wire 2 may be softened overall. Therefore, the hardness of the interior of the wire 2 also decreases, as shown in the hardness distribution H2a in Figure 17.
[0080] On the other hand, the temperature distribution Tb in Fig. 15 is a temperature at which a hardness distribution substantially similar to the hardness distribution H1 previously imparted to the wire 2 is maintained after annealing, as in the hardness distribution H2b in Fig. 17. When such a temperature distribution Tb is used, there is a possibility that the tensile residual stress in the inner diameter side portion IP cannot be sufficiently eliminated, as in the residual stress distribution σ2b in Fig. 16.
[0081] In this way, when annealing is performed with a uniform temperature distribution within the cross section of the wire 2, it is difficult to simultaneously reduce the tensile residual stress caused by coiling and maintain the hardness distribution previously imparted to the wire 2.
[0082] In contrast, when AC current heating is used, i.e., when annealing is performed with the temperature distribution T shown in FIG. 8 , it is possible to heat the surface layer of the wire 2 at a higher temperature than the interior. Therefore, while sufficiently reducing the tensile residual stress, it is possible to maintain the hardness distribution (first layer L1 and second layer L2) previously imparted to the wire 2 after annealing, for example, as shown by hardness distribution H2c in FIG. 18 . If the temperature distribution T is increased overall to enhance the effect of reducing the tensile residual stress, the hardness of the second layer L2 of the inner diameter side portion IP may decrease, as shown by hardness distribution H2d. However, even in this case, the heating temperature near the axis X2 is sufficiently low, so it is possible to maintain the hard first layer L1.
[0083] In this embodiment, the wire 2 after shot peening also has a residual stress distribution similar to the residual stress distribution σ3 in Fig. 7. That is, the peak (first peak) of the compressive residual stress in the inner diameter side portion IP is equivalent to the peak (second peak) of the compressive residual stress in the outer diameter side portion OP. In addition to the above, this embodiment can also achieve the same effects as the first embodiment.
[0084] 1...coil spring, 2...wire, X1...coil axis, X2...wire axis, IP...inner diameter side portion, OP...outer diameter side portion, DX...axial direction, DR...radial direction, Dθ...circumferential direction, L1...first layer, L2...second layer, σ, σ1, σ2, σ3...residual stress distribution, H...hardness distribution, T...temperature distribution, 100...heating device, 5...conductor, 6...ferromagnetic material.
Claims
1. A method for manufacturing a coil spring, comprising: forming a wire into a spiral shape; attaching first and second terminals to the wire, the first and second terminals being connected to a power source capable of supplying alternating current; and passing an alternating current through the wire through the first and second terminals to heat the wire with a temperature distribution in which the temperature of the inner diameter side portion of the wire is higher than the temperature of the outer diameter side portion; wherein, after the forming and before the heating, the inner diameter side portion of the wire has a higher tensile residual stress than the outer diameter side portion, and the heating reduces the tensile residual stress of the inner diameter side portion and reduces the hardness of the inner diameter side portion below the hardness of the outer diameter side portion.
2. The method for manufacturing a coil spring according to claim 1, further comprising: imparting compressive residual stress to the inner diameter side portion and the outer diameter side portion by shot peening the wire after the heating.
3. A method for manufacturing a coil spring as set forth in claim 1, wherein in the temperature distribution, the temperature of the wire shaft is lower than the temperatures of the inner diameter side portion and the outer diameter side portion.
4. A method for manufacturing a coil spring according to any one of claims 1 to 3, further comprising arranging an electrically floating conductor inside the wire formed into a spiral shape, and the heating is carried out with the conductor in place.
5. The method for manufacturing a coil spring according to any one of claims 1 to 3, further comprising arranging a ferromagnetic body on the outside of the wire formed into a spiral shape, and the heating is carried out with the ferromagnetic body in place.
Citation Information
Patent Citations
Hole inner finish machining method and device
JP1993329770A