Cellulose acylate film

The cellulose acylate film with a saponified surface layer addresses dew condensation and clouding issues, maintaining transparency and reducing carbon dioxide permeability, making it suitable for agricultural use by employing a specific acyl group substitution and molecular weight range in its composition and manufacturing process.

WO2024204404A1PCT designated stage expired Publication Date: 2024-10-03FUJIFILM CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012360
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Cellulose acylate films used in agricultural greenhouses suffer from dew condensation and clouding, leading to a decrease in transparency, which affects their optical and agricultural applications.

Method used

A cellulose acylate film with a base layer containing cellulose acylate and polyester, and a surface layer made of saponified cellulose acylate, where the acylate has an acyl group substitution degree between 2.50 and 3.00, and the polyester has a weight average molecular weight between 50,000 and 1,000,000, is developed. The film is manufactured using a cooling gelation method and saponification process to create a surface layer with a thickness of 0.20 μm to 10.00 μm, enhancing moisture permeability and reducing equilibrium water content.

Benefits of technology

The film effectively prevents dew condensation and clouding, maintaining high transparency and reducing carbon dioxide permeability, making it suitable for agricultural applications while ensuring high durability and moisture control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012360_03102024_PF_FP_ABST
    Figure JP2024012360_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a cellulose acylate film capable of preventing condensation and fogging and suppressing deterioration of transparency. The cellulose acylate film (10) is provided with a base layer (12) and a surface layer (14). The surface layer (14) is formed by saponification of the surface of a base film (20). The cellulose acylate film (10) contains cellulose acylate and polyester. The cellulose acylate has a degree of acyl group substitution in the range of 2.50-3.00. The polyester is represented by a specific formula and has a weight-average molecular weight in the range of 50,000-1,000,000 inclusive.
Need to check novelty before this filing date? Find Prior Art

Description

Cellulose acylate film

[0001] The present invention relates to a cellulose acylate film.

[0002] Cellulose acylate films, typified by cellulose acetate films, are highly transparent and moisture permeable, and therefore are used not only for optical applications such as films for polarizing plates, but also as agricultural materials such as agricultural greenhouses (see Patent Document 1 below).

[0003] International Publication No. 2016 / 103898

[0004] However, the technique disclosed in Patent Document 1 has a problem in that minute water droplets adhere to the surface of the cellulose acylate film, causing condensation and cloudiness, resulting in a decrease in transparency.

[0005] The present invention has been made in view of the above-mentioned background, and has as its object to provide a cellulose acylate film which is capable of preventing condensation and clouding and suppressing a decrease in transparency.

[0006] In order to solve the above-mentioned problems, the cellulose acylate film of the present invention comprises a base layer containing cellulose acylate and a polyester, and a surface layer provided on the base layer, wherein the surface layer is a saponified layer formed by saponifying the surface of a film-like substrate containing cellulose acylate and a polyester, and the base layer is a non-saponified layer of the substrate that has not been saponified, wherein the cellulose acylate has an acyl group substitution degree in the range of 2.50 to 3.00, and the polyester has a weight average molecular weight in the range of 50,000 to 1,000,000, and the cellulose acylate film contains at least one of a compound represented by the following general formula (1) and a compound represented by the following general formula (2): In general formula (1), R1 and R2 are the same or different alkyl groups, and n is an integer of 1 or more. In general formula (2), R3 is an alkyl group, and n is an integer of 1 or more.

[0007] In general formula (1), it is preferable that R1 is a residue derived from a diol having 2 to 6 carbon atoms, and R2 is a residue derived from a dicarboxylic acid having an aliphatic group having 2 to 6 carbon atoms.

[0008] In general formula (1), it is preferable that there are two or more types of R1 and / or R2.

[0009] In general formula (2), R3 preferably has 2 to 6 carbon atoms.

[0010] The thickness of the surface layer is preferably in the range of 0.20 μm to 10.00 μm.

[0011] The ratio of the polyester to the cellulose acylate is preferably in the range of 20 parts by mass to 120 parts by mass.

[0012] The cellulose acylate is preferably cellulose acetate.

[0013] The haze is preferably 5% or less.

[0014] It is preferable that the equilibrium moisture content is 1.5% or less.

[0015] According to the present invention, it is possible to provide a cellulose acylate film which is capable of preventing condensation and clouding and suppressing a decrease in transparency.

[0016] While the present invention has been described with reference to exemplary embodiments, it is to be understood that the invention is not limited to the disclosed exemplary embodiments and is not to be limited to the disclosed exemplary embodiments.

[0017] 1, a cellulose acylate film 10 includes a base layer 12 and a surface layer 14 provided on the surface (in this embodiment, on both the front and back surfaces) of the base layer 12. The cellulose acylate film 10 is produced through a film-forming step 30 for forming a base film 20 (base material) and a saponification step 40 for saponifying the surface of the base film 20.

[0018] In the film forming process 30, first, a dope is produced by dissolving cellulose acylate and an additive such as polyester in a solvent, such as methylene chloride or an alcohol.

[0019] Next, the dope is cast onto a support to form a cast film. A drum or a band is used as the support, and the dope is cast onto the circumferential surface of the rotating drum or the surface of the traveling band to form a cast film. At least the circumferential surface of the drum or at least the surface of the band is preferably made of metal, and preferably has a temperature control mechanism for adjusting the circumferential surface or surface to a predetermined constant temperature. When the support is a drum, the temperature control mechanism can adjust the temperature of the circumferential surface of the drum. When the support is a band, the temperature of the surface of the band can be indirectly adjusted by adjusting the temperature of the circumferential surface of the roller on which the support travels.

[0020] The solution casting method is roughly divided into a drying and gelling method and a cooling and gelling method depending on the method of solidifying the casting film. In the drying and gelling method, the casting film is dried to a desired dryness level, and the casting film is gelled and solidified by this drying. That is, the casting film is dried and solidified to such an extent that the wet film can be transported after peeling. Drying is usually performed by blowing dry air onto the casting film. Since solidifying the casting film by drying takes a longer time than solidifying by the cooling and gelling method, a band is usually used as the support instead of a drum.

[0021] On the other hand, the cooling gelation method is a method in which the casting film is actively cooled to gel it in a state where the ratio of the residual volatile matter, i.e., the residual solvent, is very high, and the gelation is continued until the casting film is hard enough to be peeled off and transported. This method can solidify the casting film in a shorter time than the drying gelation method, so a drum can be used as the support.

[0022] The casting film can be solidified by either the drying and gelling method or the cooling and gelling method, or by a combination of the drying and gelling method. Therefore, any of these methods may be employed.

[0023] However, the inventors of the present invention have found that the viscosity of the dope containing the polyester increases, especially at low temperatures. The increase in the viscosity of the dope at low temperatures, specifically the storage modulus of the dope, is due to the interaction between the cellulose acylate and the polyester, and can be appropriately adjusted by the concentration and temperature of the dope. It has been found that the dope temperature of 0°C or less is particularly effective. Therefore, it is preferable to adopt a cooling gelation method for solidifying the casting film.

[0024] Furthermore, by combining the dope and the cooling gelling method, even a thick casting film can be quickly and easily gelled, so that a relatively thick base film 20 (cellulose acylate film 10) can be produced. Furthermore, by using a drum as a support in the cooling gelling method, the casting film can be quickly peeled off and dried from both sides of the film, so that even a thick film can be produced efficiently.

[0025] After the dope is produced, the casting film is formed, and the casting film is solidified to a degree that allows the casting film to be peeled off and transported, and then the casting film is continuously peeled off from the support by using a peeling roller or the like. Then, the peeled casting film is dried. In this way, the base film 20 is formed.

[0026] The base film 20 formed in the film-forming process 30 is transported to the saponification process 40. In the saponification process 40, the surface of the base film 20 is saponified by a coating method or an immersion method. In the coating method, for example, an alkaline solution is applied as a saponifying solution to the surface of the base film 20 (in this embodiment, both the front and back surfaces), and the base film 20 coated with the alkaline solution is heated and washed. The saponifying solution contains isopropyl alcohol.

[0027] In the immersion saponification method, the base film 20 is immersed in an alkaline aqueous solution as a saponifying solution, followed by washing. Examples of the alkaline aqueous solution include a sodium hydroxide (NaOH) aqueous solution and a potassium hydroxide (KOH) aqueous solution. The saponifying solution contains propylene glycol monomethyl ether. Subsequently, the base film 20 is neutralized with an acid or an acid aqueous solution as a neutralizing solution, and then washed again and dried. In this embodiment, both sides of the base film 20 are saponified. However, a protective film may be laminated on the back side of the base film 20 to prevent saponification of the back side of the base film 20, so that only the front side is saponified.

[0028] In the saponification step 40, the surfaces of the base film 20 (both the front and back surfaces in this embodiment) are saponified, whereby the saponified portions become the above-mentioned surface layer 14 and the non-saponified portions become the above-mentioned base layer 12, thereby producing a cellulose acylate film 10 having the surface layer 14 and the base layer 12. In this manner, the surface layer 14 of the cellulose acylate film 10 is a saponified layer formed by saponifying the surface of the base film 20. The base layer 12 of the cellulose acylate film 10 is a non-saponified layer of the base film 20 that has not been saponified.

[0029] In the present embodiment, an example has been described in which the cellulose acylate film 10 is produced by saponifying both sides of the substrate film 20 to provide the surface layer 14 on both sides of the base layer 12. However, a cellulose acylate film having the surface layer 14 on one side of the base layer 12 may also be produced by saponifying one side of the substrate film 20. Thus, a cellulose acylate film having the surface layer 14 on one side of the base layer 12 is also included in the cellulose acylate film of the present invention. The cellulose acylate film 10 of the present invention, which has the surface layer 14 on both sides, does not become cloudy even when used in a high-temperature, high-humidity environment, and has high transparency. Providing the surface layer 14 on one side can suppress clouding and condensation on the side used as an agricultural material, and also makes it easier to provide another functional layer on the side not having the surface layer 14.

[0030] <Cellulose Acylate Film> The thickness of the cellulose acylate film 10 is not particularly limited, but is preferably in the range of 10 μm to 500 μm, more preferably 15 μm to 300 μm, and even more preferably 20 μm to 200 μm. Although it varies depending on the application, for example, when used as an agricultural material, the thickness is preferably in the range of 80 μm to 300 μm.

[0031] The cellulose acylate film 10 preferably has an equilibrium moisture content of 1.5% or less. The equilibrium moisture content is the moisture content in a material at equilibrium in air at a constant temperature and humidity. In this embodiment, the equilibrium moisture content is 1.5% or less in an environment of 25°C and 50% relative humidity. The equilibrium moisture content can be determined by measuring a sample of the cellulose acylate film 10 using a Karl Fischer moisture meter (e.g., AQ-2200, manufactured by Hiranuma Sangyo Co., Ltd.) after conditioning the sample for 24 hours or more at 25°C and 50% relative humidity, and dividing the measured mass of moisture in the sample by the mass of the sample. By maintaining the equilibrium moisture content within the above range, carbon dioxide permeability can be reduced, making the film suitable for use as an agricultural material. In other words, covering agricultural crops with the cellulose acylate film 10 can prevent carbon dioxide, necessary for crop growth, from escaping from the crop growth space. Although the water content tends to increase when the surface layer 14 (saponified layer) is provided, the cellulose acylate film 10 of the present invention can be suitably used as an agricultural material by reducing the carbon dioxide permeability by making the saponified layer have a certain thickness and by controlling the equilibrium water content within the above range. Furthermore, by controlling the equilibrium water content within the above range, film elongation due to high humidity or condensation during use as an agricultural material is suppressed, and sagging or the like is less likely to occur when the film is stretched as an agricultural material. The equilibrium water content is preferably 0.1% to 1.0%, more preferably 0.2% to 0.9%.

[0032] The cellulose acylate film 10 preferably has a moisture permeability of 100 g / m2·day (24 h) or more at a temperature of 40°C and a relative humidity of 90% (hereinafter, relative humidity is referred to as RH (relative humidity)). The moisture permeability is determined in accordance with Japanese Industrial Standards JIS Z0208:1976, Condition B (temperature of 40°C, 90% RH). The cellulose acylate film 10, being formed from cellulose acylate and polyester, has high moisture permeability, generally ranging from 300 g / m2·day to 1200 g / m2·day. In addition to the above-mentioned equilibrium moisture content, this high moisture permeability allows the cellulose acylate film 10 to exhibit a humidity control effect while suppressing the outflow of carbon dioxide. Furthermore, the cellulose acylate film 10 has high antifogging properties, suppressing condensation and dripping of condensed water. Therefore, for example, when a space for growing agricultural crops is formed using the cellulose acylate film 10, even if excessive moisture is generated in the space, condensation on the surface of the cellulose acylate film 10 is prevented, thereby providing drip-proofing and suppressing fog in the greenhouse, etc. The moisture permeability is preferably in the range of 200 g / m2·day to 1000 g / m2·day, more preferably in the range of 300 g / m2·day to 700 g / m2·day.

[0033] Furthermore, the cellulose acylate film 10 preferably has a haze of 5% or less. The haze indicates the degree of diffusion of transmitted light and can be measured, for example, using a haze meter (NDH5000, Nippon Denshoku Industries Co., Ltd.). By suppressing the haze to a low level, transparency is improved, and, for example, when used as an agricultural material, loss of light from a light source such as sunlight can be reduced. The haze is preferably 5% or less, both in the dry film state (e.g., after 2 hours or more in an environment of 25°C and 50% relative humidity after film preparation) and in the state of use as an agricultural material (e.g., when used in a high-temperature, high-humidity environment such as 60°C and 90% relative humidity). The cellulose acylate film 10 of the present invention, having the surface layer 14 formed by saponification, has high transparency not only in the dry film state but also when used in a high-temperature, high-humidity environment. The haze is more preferably 4% or less, and particularly preferably 3% or less.

[0034] Furthermore, the thickness of the surface layer 14 of the cellulose acylate film 10 is preferably in the range of 0.20 μm or more and 10.00 μm or less. When the thickness of the surface layer is 0.20 μm or more, the water film can be easily formed, and the haze can be kept low without clouding in a high-temperature, high-humidity environment. When the thickness of the surface layer is 10.00 μm or less, the equilibrium moisture content can be kept appropriately low. The thickness of the surface layer is more preferably 0.40 μm or more and 8.00 μm or less, and even more preferably 0.50 μm or more and 6.00 μm or less.

[0035] The thickness of the surface layer 14 can be measured by the ATR method of FT-IR or by dissolving the cellulose acylate film 10 in methylene chloride and / or chloroform. In this embodiment, the thickness of the surface layer 14 is measured as follows: A sample taken from the cellulose acylate film 10 is immersed in dichloromethane for 24 hours. The remaining undissolved sample is dried, and the thickness of the dried sample is measured three times. The average of the three measurements is defined as the thickness of the surface layer 14.

[0036] The water absorption of the surface layer 14 can be reliably increased by forming the surface layer 14 as a layer containing cellulose. When the surface layer 14 is detected as a layer by the above-mentioned dichloromethane immersion method, it is understood that the surface layer 14 is formed as a layer containing cellulose. Furthermore, when, for example, only the surface is in a cellulose state due to saponification, the saponified portion is not observed as a layer by dichloromethane immersion, and it is presumed that the cellulose moiety and the cellulose acylate moiety are mixed.

[0037] The ATR method of FT-IR can be used to measure the thickness as follows. When the amount of acyl groups on the surface of the cellulose acylate film 10 facing the surface layer 14 is X and the amount of acyl groups on the surface of the cellulose acylate film 10 facing the base layer 12 is Y, the acyl group ratio calculated by X / Y is 0.7 or less, and in this embodiment, it is set to, for example, 0.3. The smaller the acyl group ratio, the fewer acyl groups there are on the surface of the surface layer 14 compared to the surface of the base layer 12, which means that more acyl groups have been saponified to hydrophilic groups during the saponification treatment of the cellulose acylate film. The thickness of the saponified layer can be determined by comparing the measurement by the ATR method of FT-IR with the thickness of the saponified layer measured by immersion in dichloromethane.

[0038] The acyl group amount X and the acyl group amount Y are determined as the spectral intensity of the acyl group determined by the attenuated total reflection (ATR) method (hereinafter referred to as the ATR method) of Fourier transform infrared spectroscopy (FT-IR, hereinafter referred to as FT-IR). Specifically, the spectral intensity of the signal of the acyl group of cellulose acylate is corrected (normalized) by the spectral intensity of a common signal of the cellulose-based polymer. For example, when TAC, which will be described later, is used as the cellulose, the acyl group is an acetyl group, and the signal of the acetyl group is at 1210 cm -1 The common signal of cellulose-based polymers is 1030 cm -1Then, the spectral intensities of the signals of the acyl groups of the cellulose acylate obtained by the correction are determined as the acyl group amount X and the acyl group amount Y. In this way, the acyl group amount X and the acyl group amount Y are indexes that can be replaced with the number of acyl groups.

[0039] As is well known, the ATR method of FT-IR is a method in which light penetrates a measurement sample to determine the spectral intensity, and the obtained spectral intensity is not that of the surface of the measurement sample in the strict sense. When a typical FT-IR ATR method is performed using a diamond prism at a measurement angle of 45 degrees, the penetration depth of light from the surface of the measurement sample is approximately 2 to 3 μm. Because the surface layer 14 of this embodiment is very thin, as described below, the reliability of the amount of acyl groups determined for the surface layer 14 decreases as the penetration depth of light increases beyond 2 μm. Therefore, it is preferable to determine the amount of acyl groups X as the spectral intensity within a depth of 2 μm from the surface on the surface layer 14 side. In this embodiment, the penetration depth of light is set to 2 μm, and the amount of acyl groups X is determined as the spectral intensity within a range of 2 μm or less from the surface on the surface layer 14 side.

[0040] Similarly, it is preferable to determine the spectral intensity within a range of 2 μm deep from the surface on the base layer 12 side as the acyl group amount Y, and this is also done in this embodiment. When a surface layer 14 is also provided on the surface on the base layer 12 side, it is preferable to determine the acyl group amount of the substrate film 20 and use this as the acyl group amount Y. If it is difficult to determine the acyl group amount Y by this method, other methods may be used, such as dissolving the cellulose acylate film 10 in methylene chloride and / or chloroform, forming a film from the solution, and determining the acyl group amount on the film surface of this film by IR.

[0041] The cellulose acylate contained in the cellulose acylate film 10 (base film 20) has acyl groups, since hydroxy groups of cellulose are esterified with carboxylic acids. The acyl substitution degree of the cellulose acylate contained in the cellulose acylate film 10 is in the range of 2.50 to 3.00, preferably in the range of 2.60 to 2.97, and more preferably in the range of 2.70 to 2.95.

[0042] The lower the degree of acyl group substitution, the higher the water absorption of the cellulose acylate film 10, which causes deformation and sagging due to elongation caused by water absorption, and also reduces the strength. Therefore, the degree of acyl group substitution of the cellulose acylate constituting the cellulose acylate film 10 is set to 2.50 or more. Furthermore, since the theoretical upper limit of the degree of acyl group substitution is 3.00, the degree of acyl group substitution is set to 3.00 or less.

[0043] By setting the degree of acyl group substitution within a relatively high range, the water absorption of the cellulose acylate film 10 can be suppressed and the equilibrium moisture content can be set within a moderate range, thereby suppressing carbon dioxide permeability and providing a film with high moisture permeability. Furthermore, a film without elongation or strength loss due to moisture content can be obtained. On the other hand, increasing the degree of acyl group substitution reduces biodegradability. However, in this embodiment, biodegradable polyesters are added to form the cellulose acylate film 10 (substrate film 20), thereby ensuring biodegradability.

[0044] The acyl group of the cellulose acylate contained in the cellulose acylate film 10 is not particularly limited and may be an acetyl group having one carbon atom or one having two or more carbon atoms. The acyl group having two or more carbon atoms may be an aliphatic group or an aryl group, such as an alkylcarbonyl ester, alkenylcarbonyl ester, aromatic carbonyl ester, or aromatic alkylcarbonyl ester of cellulose, each of which may further have a substituted group. Examples of the acyl group having two or more carbon atoms include a propionyl group, butanoyl group, pentanoyl group, hexanoyl group, octanoyl group, decanoyl group, dodecanoyl group, tridecanoyl group, tetradecanoyl group, hexadecanoyl group, octadecanoyl group, isobutanoyl group, t-butanoyl group, cyclohexanecarbonyl group, oleoyl group, benzoyl group, naphthylcarbonyl group, and cinnamoyl group. Preferred examples of the acyl group having two or more carbon atoms include a propionyl group and a butanoyl group.

[0045] The cellulose acylate contained in the cellulose acylate film 10 may have one or more types of acyl groups, but preferably at least one of them is an acetyl group. The cellulose acylate containing an acetyl group allows the cellulose acylate film 10 to easily absorb moisture, thereby improving the effect of suppressing condensation. It is also preferable for the cellulose acylate to contain a propionyl group or a butanoyl group in addition to an acetyl group. This is because the equilibrium moisture content of the cellulose acylate film 10 can be appropriately controlled. Cellulose acylate in which all the acyl groups are acetyl groups is particularly preferred, specifically cellulose acetate (triacetylcellulose (TAC)). It is also preferable for the cellulose acylate to contain a propionyl group in addition to the acetyl group, i.e., cellulose acetate propionate (CAP).

[0046] The degree of acyl group substitution can be determined by conventional methods. For example, the degree of acetylation (degree of acetyl group substitution) can be determined according to the measurement and calculation of the degree of acetylation in ASTM: D-817-91 (Test Methods for Cellulose Acetate, etc.), a standard of ASTM International (formerly known as the American Society for Testing and Materials). It can also be measured by measuring the distribution of the acylation degree (degree of acyl group substitution) using high-performance liquid chromatography. As an example of this method, the acetylation degree of cellulose acetate is measured by dissolving the sample in methylene chloride and using a Nova-Pak (registered trademark) phenyl column (manufactured by Waters Corporation) to measure the acetylation degree distribution using a linear gradient from a mixture of methanol and water (methanol:water mass ratio 8:1) to a mixture of dichloromethane and methanol (dichloromethane:methanol mass ratio 9:1) as the eluent, and the acetylation degree distribution is determined by comparison with a calibration curve of standard samples with different degrees of acetylation. These measurement methods can be found by referring to the method described in JP-A No. 2003-201301. When the cellulose acylate is sampled from the cellulose acylate film 10, the acetylation degree of the cellulose acylate is preferably measured by high performance liquid chromatography because the sample contains additives.

[0047] <Additive (Polyester)> As described above, the cellulose acylate film 10 is formed by adding a polyester as an additive when forming the base film 20. That is, the cellulose acylate film 10 (base film 20) contains a polyester in addition to cellulose acylate.

[0048] The polyester has a weight-average molecular weight Mw of 50,000 to 1,000,000, preferably 60,000 to 500,000, and more preferably 90,000 to 200,000. When the weight-average molecular weight Mw is 50,000 or more, the equilibrium water content of the cellulose acylate film 10 can be appropriately controlled, the folding endurance of the film can be improved, and effects such as reducing residual solvent and reducing the amount of elution can be preferably exhibited. When the weight-average molecular weight Mw is 1,000,000 or less, the cellulose acylate film 10 has good transparency and low haze, the polyester is easily soluble in a solvent, and when dissolved, the dope can have an appropriate viscosity characteristic.

[0049] The polyester preferably has a dispersity, expressed as Mw / Mn, which is the ratio of weight-average molecular weight Mw to number-average molecular weight Mn, in the range of 3 to 30, more preferably in the range of 4 to 25, and even more preferably in the range of 5 to 20. When the dispersity is within this range, the polyester has a wide molecular weight distribution, and therefore, when added to cellulose acylate, the polyester has good transparency and low haze, and can improve the folding endurance of the cellulose acylate film.

[0050] The polyester is preferably a biodegradable polyester. The polyester content is preferably in the range of 20 to 120 parts by mass relative to 100 parts by mass of cellulose acylate. The greater the polyester content, the greater the effect of improving folding endurance and suppressing the equilibrium moisture content of the film. On the other hand, if the polyester content exceeds the above range, the haze increases. Therefore, the polyester content in the cellulose acylate film is set within the above range. The polyester content is preferably 25 parts by mass or more, more preferably 40 parts by mass or more, even more preferably 60 parts by mass or more, and particularly preferably 70 parts by mass or more. It is more preferably 110 parts by mass or less, and particularly preferably 100 parts by mass or less.

[0051] Examples of polyesters include PBS (polybutylene succinate) and PBAS (polybutylene succinate adipate). In this embodiment, a polyester containing at least one of a compound represented by the following general formula (1) and a compound represented by the following general formula (2) is used.

[0052]

[0053]

[0054] In general formula (1), R1 and R2 are both alkyl groups and may be the same or different, and n is an integer of 1 or greater.

[0055] In general formula (1), R1 is preferably a residue derived from a diol having 2 to 6 carbon atoms, and more preferably a residue derived from a diol having 4 to 6 carbon atoms. Furthermore, in general formula (1), R2 is preferably a residue derived from a dicarboxylic acid having an aliphatic group having 2 to 6 carbon atoms. Furthermore, in general formula (1), it is more preferable that R1 and / or R2 are two or more types, i.e., the polyester added to cellulose acylate is a copolymer. This prevents the dope from becoming cloudy (described later), provides a film with high transparency and low haze, appropriately increases the viscosity of the dope at low temperatures, and allows the content of polyester in the dope to be appropriately increased, thereby appropriately suppressing the equilibrium water content and improving folding endurance.

[0056] Preferably, R1 is a residue of butanediol, and R2 is a residue of one type of succinic acid, or two types of residues, succinic acid and adipic acid. This is PBSA. Therefore, in general formula (1), it is preferable that at least one of R1 and R2 is formed by copolymerizing two or more different aliphatic groups.

[0057] The diol having 2 to 6 carbon atoms to which R1 is added is not particularly limited, and examples thereof include ethanediol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 2-methyl-1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 2,2-dimethyl-1,3-propanediol (neopentyl glycol), 1,6-hexanediol, and 1,2-hexanediol, with 1,4-butanediol being preferred. When there are two or more types of R1, the diol having 2 to 6 carbon atoms to which R1 is added is preferably 1,4-butanediol or ethanediol.

[0058] The dicarboxylic acid having an aliphatic group with 2 to 6 carbon atoms to which R2 is added is not particularly limited, and examples thereof include succinic acid, glutaric acid, adipic acid, suberic acid, cyclohexanedicarboxylic acid, maleic acid, fumaric acid, etc., with succinic acid and adipic acid being preferred. When there are two or more types of R2, the dicarboxylic acid having an aliphatic group with 2 to 6 carbon atoms to which R2 is added is preferably succinic acid or adipic acid.

[0059] In general formula (2), R3 is an alkyl group, and n is an integer of 1 or more. In general formula (2), R3 preferably has 2 to 6 carbon atoms. R3 is generally called an aliphatic hydroxycarboxylic acid, and specific examples thereof include glycolic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 3-hydroxyvaleric acid, 4-hydroxyvaleric acid, and 6-hydroxycaproic acid, as well as cyclic esters of aliphatic hydroxycarboxylic acids, such as glycolide, which is a dimer of glycolic acid, and ε-caprolactone, which is a cyclic ester of 6-hydroxycaproic acid. These can be used alone or in combination of two or more.

[0060] Specific examples of polyesters to be added to the cellulose acylate film 10 will be described with reference to Table 1.

[0061]

[0062] In this embodiment, the polyester added to the cellulose acylate film 10 is additive A, B, C, D, or E shown in Table 1. Additive A is PBS, FZ71 manufactured by Mitsubishi Chemical Corporation. Additive B is PBS, FZ91 manufactured by Mitsubishi Chemical Corporation. Additive C is PBSA, FZ92 manufactured by Mitsubishi Chemical Corporation. Additives D and E are PBSA synthesized by ester polycondensation. The number-average molecular weight (Mn), weight-average molecular weight (Mw), and dispersity (Mw / Mn) of additives A to E, as well as the respective components R1 and R2, and the ratio of the two components when R2 is composed of two components (i.e., when the polyester is a copolymer (in this embodiment, a copolymer of succinate and butyrate)), are as shown in Table 1.

[0063] The molecular weights (Mw, Mn) were determined by gel permeation chromatography (GPC). Additive F is polyethylene adipate (PEA), a comparative example used for comparison with Additives A to E, and has a weight average molecular weight (Mw) of less than 50,000. For this Additive F, the number average molecular weight (Mn), weight average molecular weight (Mw), dispersity (Mw / Mn), and components R1 and R2 are as shown in Table 1. In Table 1, items that were not added are marked with "-".

[0064] <Additives (Other)> In addition to the polyesters described above, the cellulose acylate film 10 may contain plasticizers, ultraviolet absorbers, and particles serving as a so-called matting agent to prevent adhesion between cellulose acylate films 10. Examples of plasticizers include sugar ester derivatives. When used together with the polyesters described above, sugar ester derivatives can impart biodegradability and adjust the moisture permeability, water absorption, retardation, and other properties of the film. They also have the effect of improving the hardness and elastic modulus as well as physical properties such as tear strength, and the effect of reducing residual solvent and the amount of elution.

[0065] The amount of elution is the amount of components of the cellulose acylate film 10 that dissolve in water or the like, and can be measured by a food contact material test or the like. Specifically, the food contact material test can be a test for measuring the amount of migration of food contact materials under long-term storage at room temperature or below room temperature (OM2 conditions) as specified by the EU. In accordance with this migration amount measurement, the cellulose acylate film 10 is wrapped around a 50 cm 2 The entire film is immersed in 100 mL of a solution of 90% water and 10% ethanol by volume at 40° C. for 10 days and allowed to stand, after which the film sample is removed and the remaining solution is dried at 105° C. The weight of the remaining components is measured as the amount of elution. The amount of elution measured in this manner is preferably 10 mg or less, more preferably 5 mg or less.

[0066] The sugar ester derivative is a sugar derivative in which a hydroxyl group other than the anomeric carbon of the sugar forms an ester with an acid, and both monosaccharide ester derivatives and polysaccharide ester derivatives can be used. The sugar ester derivative may be a mixture of two or more compounds. Preferably, the sugar ester derivative uses two different compounds. For example, an ester derivative of sucrose can be used, and a mixture of two compounds, sucrose benzoate and sucrose acetate isobutyrate, can be used.

[0067] The content of the sugar ester derivative is preferably in the range of 1 part by mass to 15 parts by mass relative to 100 parts by mass of cellulose acylate. More preferably, it is in the range of 2 parts by mass to 10 parts by mass. When it is 1 part by mass or more, the effect of improving the hardness, elastic modulus, or durability of the cellulose acylate film can be exhibited, and a synergistic effect with the polyester can be exhibited, such as reducing the amount of residual solvent remaining in the film and reducing the amount of cellulose acylate film components dissolved in water, etc. When it is 15 parts by mass or less, the synergistic effect with the polyester can be preferably exhibited, which improves the hardness and elastic modulus as well as physical properties such as tear strength.

[0068] By adding a sugar ester derivative to cellulose acylate in addition to a specific polyester with a high molecular weight, such as PBS or PBSA, it is possible to achieve high hardness and high durability, drying properties during solution casting, and low elution amounts while maintaining the moisture permeability and water absorption properties of cellulose acylate.

[0069] The addition of a specific polyester to the sugar ester derivative increases the viscosity of the dope, especially at low temperatures. This makes it suitable for film production using a drum, which gels the dope and strips it off at high volatile content (residual solvent content). This allows for drying on both sides starting from the high volatile content, thereby significantly reducing residual solvent. In particular, when producing a film with a thickness of 200 μm or more, this improves film stripping and reduces residual solvent content, allowing for efficient film production of thick films.

[0070] The sugar ester derivative may be either a monosaccharide ester derivative or a polysaccharide ester derivative, and the cellulose acylate film 10 may contain both of these, or two or more kinds of monosaccharide ester derivatives or two or more kinds of polysaccharide ester derivatives.

[0071] The sugar may be a monosaccharide such as glucose, galactose, mannose, fructose, xylose, or arabinose, or a polysaccharide such as lactose, sucrose, nystose, 1F-fructosylnystose, stachyose, maltitol, lactitol, lactulose, cellobiose, maltose, cellotriose, maltotriose, raffinose, kestose, gentiobiose, gentiotriose, gentiotetraose, xylotriose, or galactosylsucrose. Glucose, fructose, sucrose, kestose, nystose, 1F-fructosylnystose, or stachyose is preferred, and sucrose or glucose is more preferred.

[0072] Oligosaccharides can also be used as polysaccharides. Oligosaccharides are produced by reacting starch, sucrose, or the like with an enzyme such as amylase. Examples of oligosaccharides include maltooligosaccharides, isomaltooligosaccharides, fructooligosaccharides, galactooligosaccharides, and xylooligosaccharides.

[0073] The monocarboxylic acid used to esterify all or part of the hydroxyl groups in the monosaccharide or polysaccharide structure is not particularly limited, and known aliphatic monocarboxylic acids, alicyclic monocarboxylic acids, aromatic monocarboxylic acids, etc. One type of carboxylic acid may be used, or two or more types may be used.

[0074] Preferred aliphatic monocarboxylic acids include saturated fatty acids such as acetic acid, propionic acid, butyric acid, isobutyric acid, valeric acid, caproic acid, enanthic acid, caprylic acid, pelargonic acid, capric acid, 2-ethyl-hexanecarboxylic acid, undecylic acid, lauric acid, tridecylic acid, myristic acid, pentadecylic acid, palmitic acid, heptadecylic acid, stearic acid, nonadecanoic acid, arachidic acid, behenic acid, lignoceric acid, cerotic acid, heptacosanoic acid, montanic acid, melissic acid, and lacteric acid; unsaturated fatty acids such as undecylenic acid, oleic acid, sorbic acid, linoleic acid, linolenic acid, arachidonic acid, and octenoic acid; and alicyclic monocarboxylic acids such as cyclopentanecarboxylic acid, cyclohexanecarboxylic acid, and cyclooctanecarboxylic acid.

[0075] Preferred examples of aromatic monocarboxylic acids include aromatic monocarboxylic acids in which an alkyl group or an alkoxy group has been introduced into the benzene ring of benzoic acid, such as benzoic acid or toluic acid, and aromatic monocarboxylic acids having two or more benzene rings, such as cinnamic acid, benzilic acid, biphenylcarboxylic acid, naphthalenecarboxylic acid, or tetralincarboxylic acid, or derivatives thereof, with benzoic acid or naphthyl acid being particularly preferred.

[0076] Therefore, as the sugar ester derivative, an ester derivative of sucrose, more specifically, sucrose benzoate (sucrose benzoate, SB), sucrose acetate isobutyrate (sucrose acetate isobutyrate, SAIB), etc., can be preferably used. Specifically, these can be those shown in the following formula (3). In formula (3), R in sucrose benzoate is benzoyl or H, and the average degree of substitution is 5.7. In formula (3), R in sucrose acetate isobutyrate is acetyl and isobutyryl, with the ratio of acetyl to isobutyryl being 2 / 6.

[0077]

[0078] As a commercially available product, "Monopet (registered trademark) SB" (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) can be used as sucrose benzoate.

[0079] The safety of each sugar ester derivative is described in the following documents: Journal of the Society of Organic Synthetic Chemistry, Vol. 21 (1963) No. 1, p. 19-27; Dai-ichi Kogyo Seiyaku Catalog; and JP 2011-237764 A. The Dai-ichi Kogyo Seiyaku Catalog describes sugar fatty acid esters and benzoic acid esters. The safety includes not only the safety of the above substances themselves, but also the safety of their decomposition products.

[0080] As described above, in this embodiment, two types of sugar ester derivatives represented by formula (3), sucrose benzoate and sucrose acetate isobutyrate, are used.

[0081] In addition to the cellulose acylate and the additives consisting of the sugar ester derivative and polyester, other additives may be contained in the cellulose acylate film 10. In this embodiment, an ultraviolet absorber is added, and specifically, a compound represented by the following formula (4) is used.

[0082]

[0083] The additives contained in the cellulose acylate film 10, including the compound represented by formula (4), are additives mixed in the dope.

[0084] Examples and Comparative Examples Examples of the present invention and comparative examples for the present invention will be described below with reference to Tables 2, 3 and 4.

[0085]

[0086]

[0087]

[0088] In the examples and comparative examples, CA-1 to CA-4 and CAP shown in Table 2 were used as cellulose acylates. The acylation degree, number average molecular weight Mn, weight average molecular weight Mw, and dispersity Mn / Mw of each of CA-1 to CA-4 and CAP are as shown in Table 2. The CAP used was commercially available CAP482-20 (manufactured by Eastman Chemical Company, acylation degree 2.67 (acetylation degree 0.18, propionylation degree 2.49)).

[0089] In the examples and comparative examples, a base film was formed by the film-forming process 30 shown in Fig. 1. In examples 1 to 6 and comparative example 1, 2 parts by mass of a UV absorber represented by formula (4) was added. In example 8, 10 parts by mass of a sugar ester compound represented by formula (3) was added. Then, a surface layer 14 was formed on the film (cellulose acylate film) by the saponification process 40 shown in Fig. 1, and the film of the example was used.

[0090] In Examples 1 to 12, saponification was performed on both sides of the film by the following coating method. Specifically, a rolled substrate was unwound and transported, and a saponifying solution was applied to one film surface of the substrate using a coating device installed in the transport path. The saponifying solution had the following formulation. In the formulation, % represents percentage by mass: potassium hydroxide (KOH) 3.3%, isopropyl alcohol 88%, water 3.66%, propylene glycol 5%, surfactant 0.04%. The cellulose acylate film coated with the saponifying solution was guided into a heating chamber installed in the transport path and heated while being transported, and then sent to a water tank containing water and washed with water to form a surface layer.

[0091] In Examples 13 to 22, both surfaces of the substrate were saponified by the following immersion method (a method in which the substrate was immersed in a saponification solution to form a surface layer). Specifically, the substrate was immersed in a 1.5 mol / L NaOH solution containing water and propylene glycol monomethyl ether in a ratio of 8:2, with the liquid temperature and immersion time adjusted. Thereafter, the substrate was immersed in pure water at 25°C for 15 seconds as a first cleaning step, neutralized by immersion in a 0.3 mol / L sulfuric acid aqueous solution (HSO aq) at 25°C for 15 seconds as a neutralization step, and then immersed in pure water at 25°C for 15 seconds as a second cleaning step. The substrate surface was then drained with an air knife, and then dried in an environment at 100°C for 60 seconds as a drying step to form a surface layer.

[0092] In Examples 23 and 24, both surfaces of the substrate were saponified by the following immersion method (a method in which the substrate was immersed in a saponification solution to form a surface layer). Specifically, the substrate was immersed in a 1.5 mol / L NaOH solution containing water and ethyl alcohol at a ratio of 75:25, with the liquid temperature and immersion time adjusted. Thereafter, the substrate was immersed in pure water at 25°C for 15 seconds as a first cleaning step, neutralized by immersion in a 0.3 mol / L sulfuric acid aqueous solution (HSO aq) at 25°C for 15 seconds as a neutralization step, and then immersed in pure water at 25°C for 15 seconds as a second cleaning step. The substrate surface was then drained with an air knife, and then dried in an environment at 100°C for 60 seconds as a drying step to form a surface layer.

[0093] On the other hand, a comparative film was prepared by not forming the surface layer 14. The type and amount (parts by mass) of cellulose acylate, the type and amount (parts by mass) of additives, the thickness of the film, and the thickness of the surface layer (on one side) in the examples and comparative examples are as shown in Table 3.

[0094] For each of the films of the Examples and Comparative Examples, the haze of the dry film (%), the haze in a high-temperature and high-humidity environment (%), the elastic modulus, the folding strength (folding times), the equilibrium moisture content (%), and the moisture permeability (g / m 2  The haze of the dry film, the haze in a high-temperature, high-humidity environment, the elastic modulus, the folding strength, the equilibrium water content, the moisture permeability, the evaluation of the haze in a high-temperature, high-humidity environment, and the evaluation of the water film (formability) are shown in Table 4.

[0095] In Table 4, the haze was measured using a haze meter (NDH5000, Nippon Denshoku Industries Co., Ltd.). The haze of the dry film was measured after the film had been prepared and left in an environment of 25°C and 50% relative humidity for at least 2 hours. The haze in a high-temperature, high-humidity environment was measured after the film had been stored in an environment of 60°C and 90% relative humidity for at least 24 hours as a storage test in a high-temperature, high-humidity environment.

[0096] The evaluation of cloudiness was carried out by visually inspecting the film after storage in a high-temperature, high-humidity environment (after 24 hours or more in an environment of 60°C and 90% relative humidity). Transparent films were evaluated as "A", films with partial cloudiness on the surface were evaluated as "B", and films with cloudiness over the entire surface were evaluated as "C".

[0097] The water film was evaluated by placing a 5 cm x 30 cm film in a 40°C water bath so that the angle between the film and the water surface was 45 degrees and leaving it for 10 minutes. When a water film was formed on the film, it appeared transparent, while when it was not formed, it appeared cloudy. Using this, the film was evaluated based on the area percentage of the water film-formed portion and visibility. Specifically, when the water film formed in the range of 80% to 100% and the entire film appeared transparent, the evaluation was given an "A." When the water film formed in the range of 30 to 80% and most of the film appeared transparent, the evaluation was given a "B." When the water film formed in the range of 30% or less and the entire film appeared opaque, the evaluation was given a "C."

[0098] The tensile modulus was measured in accordance with Japanese Industrial Standard JIS K7161:2014. Specifically, a total of eight test pieces, each 150 mm long and 15 mm wide, were prepared from the film by cutting out the test piece in an angle of 45°. The test pieces were stretched at a chuck length of 100 mm and a tensile speed of 200 mm / min under an environment of 25°C and 60% relative humidity, and the strains at elongations of 0.1% and 0.5% were measured. The moduli were calculated from the slopes of the strain at two points, and the average value was used as the final modulus, as shown in Table 4. A tensile tester (manufactured by A&D Co., Ltd.) was used as the measuring machine.

[0099] The folding endurance indicates durability against folding, and was determined by the MIT test method. Specifically, a test piece of cellulose acylate film having a width of 15 mm and a length of 110 mm was subjected to a load of 9.8 N and a bending angle of 135 degrees on the left and right sides with a curvature radius of R0.38 using a No. 530 MIT type folding endurance tester manufactured by Toyo Seiki Co., Ltd., and the number of times until breakage was determined.

[0100] The equilibrium moisture content is the moisture content in a state where the moisture content in a material reaches equilibrium in air at a constant temperature and humidity. A sample of cellulose acylate film was conditioned for 24 hours in an environment of 25°C and a relative humidity of 50%, and then the moisture content was determined by dividing the mass of moisture in the sample measured using a Karl Fischer moisture meter (AQ-2200, manufactured by Hiranuma Sangyo Co., Ltd.) by the mass of the sample.

[0101] The moisture permeability indicates the amount of water vapor that passes through a unit area of ​​a film-like material in a certain period of time, and was determined in an environment of 40°C and a relative humidity of 90% in accordance with Japanese Industrial Standard JIS Z-0208. Note that in Figures 2 to 4, items that were not added, not measured (measurable), or not evaluated (evaluable) are marked with "-".

[0102] From Table 4, it was confirmed that the films of the examples, i.e., the cellulose acylate film 10 of the present invention, have excellent water film forming properties, are highly effective in preventing cloudiness (condensation and fogging) particularly under high humidity conditions, and can maintain high transparency. Thus, the cellulose acylate film 10 of the present invention can be suitably used as an agricultural material because it can prevent condensation and fogging and maintain high transparency.

[0103] As shown in Figures 2 and 3, when the cellulose acylate film 10 of the present invention is used as an agricultural material, it can be used as a cover for covering a crop 50 and its culture medium 52. In Figures 2 and 3, the cellulose acylate film 10 is unwound from a roll 54 and stretched over support rollers 56 and 58 to cover the crop 50 and the culture medium 52, thereby forming a growing space 60 for the crop 50. Carbon dioxide necessary for the growth of the crop 50 is supplied to the growing space 60 from a carbon dioxide supplying device 62. The support rollers 56 and 58 move up and down between the state shown in Figure 2 and the state shown in Figure 3 in accordance with the growth of the crop 50. This allows carbon dioxide to be efficiently supplied into the growing space 60 while suppressing the amount of carbon dioxide supplied.

[0104] As described above, the provision of the surface layer 14 (see FIG. 1 ) on the cellulose acylate film 10 prevents condensation and fogging, thereby maintaining high transparency. Furthermore, moisture contained in the crops 50 and the culture medium 52 tends to cause higher humidity inside the cultivation space 60 than outside the cultivation space 60, which makes condensation and fogging more likely to occur on the surface of the cellulose acylate film 10 facing the cultivation space 60. Therefore, when the surface layer 14 is provided on only one side of the cellulose acylate film 10, the surface layer 14 is used facing the cultivation space 60. This more reliably prevents condensation and fogging, thereby realizing a favorable cultivation environment for the crops 50.

[0105] As described above, the cellulose acylate film 10 can reduce the carbon dioxide permeability by keeping the equilibrium moisture content low. Therefore, by covering the growth space 60 with the cellulose acylate film 10 having a low equilibrium moisture content, specifically, 1.5% or less, it is possible to suppress the outflow of carbon dioxide.

[0106] Furthermore, when the cellulose acylate film 10 of the present invention is used as an agricultural material, it has good folding strength and is highly durable during repeated unwinding and winding when it is unrolled from a roll, wound around, or passed between support rollers or transported, which is preferable.

[0107] REFERENCE SIGNS LIST 10 Cellulose acylate film 12 Base layer 14 Surface layer 20 Base film (base material) 30 Film-forming process 40 Saponification process 50 Agricultural crop 52 Culture medium 54 Film roll 56, 58 Support rollers 60 Growing space 62 Carbon dioxide supply device

Claims

1. A cellulose acylate film comprising a base layer containing cellulose acylate and a polyester, and a surface layer provided on the base layer, wherein the surface layer is a saponified layer formed by saponifying the surface of a film-like substrate containing the cellulose acylate and the polyester, the base layer is a non-saponified layer of the substrate that has not been saponified, the cellulose acylate has an acyl group substitution degree in the range of 2.50 to 3.00, and the polyester has a weight average molecular weight in the range of 50,000 to 1,000,000, and contains at least one of a compound represented by the following general formula (1) and a compound represented by the following general formula (2): In the general formula (1), R1 and R2 are the same or different alkyl groups, and n is an integer of 1 or more. In the general formula (2), R3 is an alkyl group, and n is an integer of 1 or more.

2. The cellulose acylate film according to claim 1, wherein in the general formula (1), R1 is a residue derived from a diol having 2 to 6 carbon atoms, and R2 is a residue derived from a dicarboxylic acid having an aliphatic group having 2 to 6 carbon atoms.

3. The cellulose acylate film according to claim 2, wherein, in the general formula (1), R1 and / or R2 are two or more kinds.

4. The cellulose acylate film according to claim 1, wherein in the general formula (2), R3 has 2 to 6 carbon atoms.

5. The cellulose acylate film according to any one of claims 1 to 4, wherein the thickness of the surface layer is in the range of 0.20 µm to 10.00 µm.

6. The cellulose acylate film according to claim 5, wherein the ratio of said polyester to said cellulose acylate is in the range of 20 parts by weight to 120 parts by weight.

7. The cellulose acylate film according to claim 6, wherein the cellulose acylate is cellulose acetate.

8. The cellulose acylate film according to claim 7, which has a haze of 5% or less.

9. The cellulose acylate film according to claim 8, which has an equilibrium moisture content of 1.5% or less.

Citation Information

Patent Citations

  • Method for adjusting acetylation degree of cellulose acetate

    JP2003201301A

  • Cellulose acylate film, polarizing plate, and liquid crystal display device

    JP2011237764A

  • Film for agricultural house and agricultural house

    WO2016103898A1

  • Cellulose acylate film, manufacturing method therefor, and optical film using the film

    JP2004292696A

  • Cellulose ester film, retardation film, polarizing plate and liquid crystal display apparatus

    JP2010242050A