Layered body
The laminate structure addresses the issue of cracking in base materials with different expansion coefficients by using a second resin layer with a lower storage modulus to absorb thermal expansion differences, ensuring structural integrity and stability in planar heaters.
Patent Information
- Application Number
- PCT/JP2024/012440
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Existing laminates used in planar heaters can develop cracks when placed between base materials with different linear expansion coefficients, leading to structural integrity issues.
A laminate structure comprising a first base material with a lower linear expansion coefficient, a second base material with a higher linear expansion coefficient, and a wiring sheet sandwiched between them, with a second resin layer having a lower storage modulus than the first resin layer, which allows for deformation and alleviates strain on the second base material, preventing cracks.
The laminate effectively prevents cracks in the base material by allowing the second resin layer to deform and absorb thermal expansion differences, maintaining structural integrity and stability.
Smart Images

Figure JP2024012440_03102024_PF_FP_ABST
Abstract
Description
Laminate
[0001] The present invention relates to a laminate.
[0002] As an example of a wiring sheet that can be used for a sheet heater, Patent Document 1 discloses a wiring sheet that includes a pseudo-sheet structure in which a plurality of conductive linear members are arranged at intervals, a cured material layer that supports the pseudo-sheet structure, and a pair of electrodes that directly contact the conductive linear members. In this wiring sheet, the cured material layer is made of a cured product of a curable adhesive, and the storage modulus of the cured material layer at 23°C is 5.0 × 10 6 Pa or more 1.0×10 10 Pa or less.
[0003] International Publication No. 2021 / 225142
[0004] The wiring sheet described in Patent Document 1 can stabilize the resistance value of the wiring. However, it has been found that when the wiring sheet described in Patent Document 1 is disposed between two substrates having different linear expansion coefficients, cracks may occur in one of the substrates.
[0005] An object of the present invention is to provide a laminate that can prevent cracks from occurring in the substrate.
[0006] [1] A laminate comprising a first substrate, a second substrate having a linear expansion coefficient higher than that of the first substrate, and a wiring sheet sandwiched between the first substrate and the second substrate, wherein the wiring sheet comprises a wiring body in which a plurality of conductive linear members are arranged at intervals, a first resin layer that directly or indirectly supports the wiring body, and a pair of electrodes in direct contact with the conductive linear members, and the first substrate or the second substrate and the wiring sheet are laminated via a second resin layer that has a storage modulus lower than that of the first resin layer.
[0007] [2] The laminate according to [1], wherein the storage modulus of the second resin layer at 23°C is 1.0 × 10 4 Pa or more, 3.0×10 5 The laminate has a modulus of elasticity of 100 Pa or less.
[0008] [3] The laminate according to [1] or [2], wherein the storage modulus of the first resin layer at 23°C is 5.0 × 10 6 Pa or more, 1.0×10 10 The laminate has a modulus of elasticity of 100 Pa or less.
[0009] [4] The laminate according to any one of [1] to [3], wherein the linear expansion coefficient of the first substrate is 0.01 × 10 -6 / ℃ or more, 10 × 10 -6 / °C or less.
[0010] [5] The laminate according to any one of [1] to [4], wherein the linear expansion coefficient of the second substrate is 50×10 -6 / ℃ or more, 100 × 10 -6 / °C or less.
[0011] [6] The laminate according to any one of [1] to [5], wherein the second base material and the wiring sheet are laminated with the second resin layer interposed therebetween.
[0012] According to one aspect of the present invention, a laminate capable of preventing cracks from occurring in a substrate can be provided.
[0013] It is a schematic diagram showing a laminate according to a first embodiment of the present invention. It is a cross-sectional view showing the II-II cross section of Fig. 1. It is a cross-sectional view showing a cross section of a laminate according to a second embodiment of the present invention.
[0014] [First embodiment] Hereinafter, the present invention will be described with reference to the drawings, taking an embodiment as an example. The present invention is not limited to the content of the embodiment. Note that in the drawings, some parts are illustrated enlarged or reduced in size for ease of explanation.
[0015] (Laminate) As shown in FIGS. 1 and 2 , the laminate 100 according to this embodiment includes a first substrate 1, a second substrate 2 having a linear expansion coefficient higher than that of the first substrate 1, and a wiring sheet 10 sandwiched between the first substrate 1 and the second substrate 2. The wiring sheet 10 includes a wiring body 3 having a plurality of conductive linear members 31 arranged at intervals, a first resin layer 4 that directly or indirectly supports the wiring body 3, and a pair of electrodes 5 in direct contact with the conductive linear members 31. The first substrate 1 or the second substrate 2 and the wiring sheet 10 are laminated via a second resin layer 6 having a storage modulus lower than that of the first resin layer 4. In FIG. 2 , the second substrate 2 and the wiring sheet 10 are laminated via the second resin layer 6. The second substrate 2 has two holes that allow electrical connection between the pair of electrodes 5 and a power source (not shown).
[0016] The inventors speculate that the laminate 100 according to this embodiment can prevent cracks from occurring in the substrates because of the following reasons. Specifically, cracks occur in the second substrate 2 due to the difference in linear expansion coefficient between the first substrate 1 and the second substrate 2. For example, when the laminate 100 is heated to a high temperature, the second substrate 2 expands more than the first substrate 1. Furthermore, because the first substrate 1 and the second substrate 2 are fixed by the wiring sheet 10 sandwiched between them, distortion occurs in the second substrate 2, resulting in cracks. In contrast, in this embodiment, the first substrate 1 or the second substrate 2 and the wiring sheet 10 are laminated via the second resin layer 6, which has a lower storage modulus than the first resin layer 4. Furthermore, the second resin layer 6 is easily deformed due to its low storage modulus. Therefore, when the laminate 100 is heated to a high temperature, the second resin layer 6 deforms, thereby alleviating distortion occurring in the second substrate 2. In this way, cracks can be prevented from occurring in the substrates.
[0017] (First substrate) The first substrate 1 can directly or indirectly support the wiring body 3. Furthermore, the first substrate 1 can protect one side of the wiring sheet 10. The linear expansion coefficient of the first substrate 1 is lower than the linear expansion coefficient of the second substrate 2. Thus, even if there is a difference in the linear expansion coefficient, according to this embodiment, it is possible to prevent cracks from occurring in the second substrate 2. The linear expansion coefficient of the first substrate 1 is 0.01 × 10 -6 / °C or more, and may be 0.1 × 10 -6 / °C or more, and may be 0.5 × 10 -6 / °C or more. The linear expansion coefficient of the first substrate 1 may be 20×10 -6 / °C or less, and preferably 10 x 10 -6 / °C or less, and more preferably 5 x 10 -6 / °C or less is particularly preferred. The linear expansion coefficient can be measured by the method described in the examples below. The conditions for measuring the linear expansion coefficient are as described below.
[0018] From the viewpoint of the strength and handleability of the laminate, resin, glass, etc. are preferred as the material of the first substrate 1. When the first substrate 1 is in the form of a film, the thickness of the first substrate 1 is not particularly limited. The thickness of the first substrate 1 is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 50 μm or more. Furthermore, the thickness of the first substrate 1 is preferably 10 mm or less, more preferably 5 mm or less, and even more preferably 3 mm or less.
[0019] (Second substrate) The second substrate 2 can directly or indirectly support the wiring body 3. Furthermore, the second substrate 2 can protect one side of the wiring sheet 10. The linear expansion coefficient of the second substrate 2 is higher than that of the first substrate 1. Thus, even if there is a difference in the linear expansion coefficient, according to this embodiment, it is possible to prevent cracks from occurring in the second substrate 2. The linear expansion coefficient of the second substrate 2 is 30×10 -6 / °C or more, and -6 / °C or more, and more preferably 60 x 10 -6 / °C or more. The linear expansion coefficient of the second substrate 2 is more preferably 200 × 10 -6 / °C or less, and -6 / °C or less, and more preferably 100 x 10 -6 / ° C. or less is more preferable. The method for measuring the linear expansion coefficient is as described below.
[0020] From the viewpoint of the handleability of the laminate and the suitability for manufacturing, a resin or the like is preferable as the material of the second base material 2. Examples of resins include polyethylene, polypropylene, polybutene, polybutadiene, polymethylpentene, polyvinyl chloride, vinyl chloride copolymer, polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, polyurethane, ethylene-vinyl acetate copolymer, ionomer resin, ethylene-(meth)acrylic acid copolymer, polystyrene, polycarbonate, cycloolefin polymer, and polyimide.
[0021] When the second substrate 2 is in the form of a film, there are no particular limitations on the thickness of the second substrate 2. The thickness of the second substrate 2 is preferably 10 μm or more, more preferably 30 μm or more, and even more preferably 50 μm or more. The thickness of the second substrate 2 is preferably 10 mm or less, more preferably 5 mm or less, and even more preferably 3 mm or less.
[0022] (Wiring Sheet) The wiring sheet 10 includes a wiring body 3, a first resin layer 4, and a pair of electrodes 5. The wiring sheet 10 is sandwiched between a first substrate 1 and a second substrate 2, and both surfaces of the wiring sheet 10 are protected by the first substrate 1 and the second substrate 2.
[0023] (Wiring Body) The wiring body 3 has a structure in which a plurality of conductive linear bodies 31 are arranged at intervals from one another. The wiring body 3 also has a structure in which a plurality of conductive linear bodies 31 are arranged in parallel.
[0024] The conductive linear body 31 may be linear or may have a wave shape in a plan view of the laminate 100. Examples of the wave shape include a sine wave, a rectangular wave, a triangular wave, and a sawtooth wave. For example, if the wiring body 3 has such a structure, breakage of the conductive linear body 31 can be suppressed when the laminate 100 is stretched in the axial direction of the conductive linear body 31.
[0025] The volume resistivity of the conductive linear body 31 is 1.0×10 -9 It is preferable that the resistance is Ω·m or more, and 3.0×10 -9 More preferably, it is 1.0×10 -8 It is more preferable that the volume resistivity of the conductive linear body 31 is 1.0×10 -3 It is preferably Ω·m or less, and 1.0×10 -4 More preferably, it is 1.0×10 -5 It is more preferable that the volume resistivity is Ω·m or less. When the volume resistivity of the conductive linear body 31 is in the above range, the surface resistance of the wiring body 3 is likely to decrease. The volume resistivity of the conductive linear body 31 is measured as follows. Silver paste is applied to the end of the conductive linear body 31 and a portion 40 mm from the end, and the resistance of the end and a portion 40 mm from the end is measured. Then, the cross-sectional area (unit: m) of the conductive linear body 31 is measured. 2 ) is multiplied by the resistance value, and the obtained value is divided by the measured length (0.04 m) to calculate the volume resistivity of the conductive linear body 31.
[0026] The cross-sectional shape of the conductive linear body 31 is not particularly limited and may be polygonal, flat, elliptical, circular, etc. From the viewpoint of compatibility with the first resin layer 4, the cross-sectional shape of the conductive linear body 31 is preferably elliptical or circular.
[0027] When the cross section of the conductive linear body 31 is circular, the diameter D (see FIG. 2 ) of the conductive linear body 31 is preferably 3 μm or more and 200 μm or less. From the viewpoints of suppressing an increase in sheet resistance and improving the heat generation efficiency and dielectric breakdown resistance characteristics of the laminate 100, the diameter D of the conductive linear body 31 is more preferably 4 μm or more, and even more preferably 5 μm or more. The diameter D of the conductive linear body 31 is more preferably 150 μm or less, even more preferably 100 μm or less, particularly preferably 50 μm or less, and extremely preferably 20 μm or less. When the cross section of the conductive linear body 31 is elliptical, the major axis is preferably in the same range as the diameter D above.
[0028] The diameter D of the conductive linear body 31 is determined by observing the conductive linear body 31 using a digital microscope, measuring the diameter of the conductive linear body 31 at five randomly selected points, and averaging the measured values.
[0029] The spacing L (see FIG. 2 ) between the conductive linear bodies 31 is preferably 0.3 mm or more, more preferably 0.5 mm or more, even more preferably 0.8 mm or more, and particularly preferably 1.5 mm or more. Furthermore, the spacing L between the conductive linear bodies 31 is preferably 50 mm or less, more preferably 30 mm or less, even more preferably 20 mm or less, and particularly preferably 5 mm or less. When the spacing between the conductive linear bodies 31 is within the above range, the conductive linear bodies 31 are relatively densely packed, thereby improving the functionality of the laminate 100, such as maintaining low resistance of the wiring body 3.
[0030] The interval L between the conductive linear bodies 31 is measured by, for example, observing the conductive linear bodies 31 of the wiring body 3 using a digital microscope and measuring the interval between two adjacent conductive linear bodies 31. The interval between two adjacent conductive linear bodies 31 is the length along the direction in which the conductive linear bodies 31 are arranged, and is the length between opposing portions of the two conductive linear bodies 31 (see FIG. 2). When the conductive linear bodies 31 are arranged at uneven intervals, the interval L is the average value of the intervals between all adjacent conductive linear bodies 31.
[0031] The conductive linear body 31 may be formed by any method, including etching, screen printing, and inkjet printing. However, a linear body containing a metal wire (hereinafter also referred to as a "metal wire linear body") is preferred. Metal wire has high thermal conductivity, high electrical conductivity, and easy handling. Metal wire linear bodies can significantly reduce resistance, and even if the diameter of the metal wire linear body is extremely small, the current required for generating heat in the laminate 100 can still be passed through. This makes the conductive linear body 31 less visible. In other words, using a metal wire linear body as the conductive linear body 31 can reduce the resistance value of the wiring body 3 while improving light transmittance. Furthermore, the laminate 100 can easily generate heat quickly. Furthermore, as described above, a linear body with a small diameter can be easily obtained. In addition to metal wire linear bodies, examples of the conductive linear body 31 include linear bodies containing carbon nanotubes and linear bodies formed by applying a conductive coating to a thread.
[0032] The metal wire linear body may be a linear body consisting of a single metal wire, or a linear body consisting of multiple twisted metal wires. Examples of metal wires include wires containing metals such as copper, aluminum, tungsten, iron, molybdenum, nickel, titanium, silver, and gold, or alloys containing two or more metals (e.g., steels such as stainless steel and carbon steel, brass, phosphor bronze, zirconium-copper alloys, beryllium copper, iron-nickel, nichrome, nickel-titanium, Kanthal, Hastelloy, and rhenium-tungsten). The metal wire may be plated with gold, tin, zinc, silver, nickel, chromium, nickel-chromium alloys, solder, or the like, and may be surface-coated with a carbon material or polymer, as described below. Wires containing one or more metals selected from tungsten, molybdenum, and alloys containing these metals are particularly preferred from the viewpoint of low volume resistivity. Examples of metal wires include metal wires coated with a carbon material. When a metal wire is coated with a carbon material, the metallic luster is reduced, making it easier to make the metal wire less noticeable. Furthermore, when a metal wire is coated with a carbon material, metal corrosion is also suppressed. Examples of carbon materials that can be used to coat a metal wire include amorphous carbon such as carbon black, activated carbon, hard carbon, soft carbon, mesoporous carbon, and carbon fiber; graphite, fullerene, graphene, and carbon nanotubes.
[0033] The conductive linear body 31 may be a linear body in which a conductive coating is applied to a thread. Examples of the thread include threads spun from resins such as nylon or polyester. Examples of the thread include threads made of metal fiber, carbon fiber, or ion-conductive polymer fiber. Examples of the conductive coating include coatings made of metal, conductive polymer, or carbon material. The conductive coating can be formed by plating, vapor deposition, or the like. A linear body in which a conductive coating is applied to a thread can improve the conductivity of the linear body while maintaining the flexibility of the thread. In other words, it becomes easier to reduce the resistance of the wiring body 3.
[0034] (First Resin Layer) The first resin layer 4 directly or indirectly supports the wiring body 3. Furthermore, the first resin layer 4 can stabilize the resistance value of the wiring body 3. That is, the first resin layer 4 can fix the conductive linear body 31, stabilize the contact between the conductive linear body 31 and the electrode 5, and make it difficult for the resistance value to increase. From the viewpoint of stabilizing the resistance value of the wiring body 3, the storage modulus of the first resin layer 4 at 23°C is 5.0 × 10 6 Pa or more, 1.0×10 10 From the same viewpoint, the storage modulus of the first resin layer 4 at 23° C. is preferably 5.0×10 Pa or less. 7 Pa or more, and more preferably 5.0 × 10 8 The storage modulus of the first resin layer at 23°C is more preferably 7.0 × 10 Pa or more. 9 Pa or less, and more preferably 4.0 × 10 9 From the same viewpoint, the storage modulus of the first resin layer 4 at 105° C. is more preferably 5.0×10 Pa or less. 7 Pa or more, and 8 The storage modulus of the first resin layer 4 at 105°C is more preferably 7.0 × 10 Pa or more. 9 Pa or less, and 9 It is more preferable that the storage modulus is not more than Pa. The storage modulus can be measured by the method described in the examples below.
[0035] The thickness of the first resin layer 4 is not particularly limited. The thickness of the first resin layer 4 may be equal to or greater than the diameter D of the conductive linear body 31, or may be less than the diameter D of the conductive linear body 31. When the thickness of the first resin layer 4 is equal to or greater than the diameter D of the conductive linear body 31, the wiring body 3 can be contained within the first resin layer 4. When the thickness of the first resin layer 4 is less than the diameter D of the conductive linear body 31, the wiring body 3 is exposed from the first resin layer 4. Furthermore, when the wiring body 3 is exposed from the first resin layer 4, the wiring body 3 may be exposed on the side of the first substrate 1 or the side of the second substrate 2. The thickness of the first resin layer 4 is preferably 1 μm or greater, more preferably 5 μm or greater, and even more preferably 10 μm or greater. The thickness of the first resin layer 4 is preferably 100 μm or less, more preferably 50 μm or less, and even more preferably 30 μm or less.
[0036] From the viewpoint of setting the storage modulus within the above range, the first resin layer 4 is preferably a layer made of a cured product of a curable adhesive. Examples of the curable adhesive include a thermosetting adhesive that cures with heat and an energy ray-curable adhesive. Examples of the energy ray include ultraviolet light, visible energy rays, infrared rays, and electron beams. Note that "energy ray curing" also includes thermal curing by heating using energy rays.
[0037] The curable adhesive preferably contains a thermosetting resin. Examples of thermosetting resins include, but are not limited to, epoxy resins, phenolic resins, melamine resins, urea resins, polyester resins, urethane resins, acrylic resins, benzoxazine resins, phenoxy resins, amine compounds, and acid anhydride compounds. These resins can be used alone or in combination. Among these, epoxy resins, phenolic resins, melamine resins, urea resins, amine compounds, and acid anhydride compounds are preferred because they are suitable for curing using an imidazole curing catalyst. In particular, epoxy resins, phenolic resins, mixtures thereof, or mixtures of epoxy resins with at least one selected from the group consisting of phenolic resins, melamine resins, urea resins, amine compounds, and acid anhydride compounds are preferred because they exhibit excellent curability. Epoxy resins are preferred.
[0038] As the epoxy resin, a cyclic one such as an aromatic epoxy resin or an alicyclic epoxy resin is preferred from the viewpoint of increasing the storage modulus of the first resin layer 4. An epoxy resin having a flexible segment such as an oxyalkylene chain tends to decrease the storage modulus of the first resin layer 4.
[0039] The energy ray-curable adhesive preferably contains an energy ray-curable resin, such as a compound having at least one polymerizable double bond in the molecule, and preferably an acrylate compound having a (meth)acryloyl group.
[0040] Examples of the acrylate compounds include dicyclopentadiene diacrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol monohydroxypenta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,4-butylene glycol di(meth)acrylate, and 1,6-hexanediol di(meth)acrylate. acrylate and other linear aliphatic skeleton-containing (meth)acrylates; cyclic aliphatic skeleton-containing (meth)acrylates such as dicyclopentanyl di(meth)acrylate; polyalkylene glycol (meth)acrylates such as polyethylene glycol di(meth)acrylate; oligoester (meth)acrylates, urethane (meth)acrylate oligomers, epoxy-modified (meth)acrylates, polyether (meth)acrylates other than polyalkylene glycol (meth)acrylates, and itaconic acid oligomers.
[0041] The weight average molecular weight (Mw) of the energy ray curable resin is preferably 100 or more, more preferably 300 or more. The weight average molecular weight is preferably 30,000 or less, more preferably 10,000 or less. The weight average molecular weight in this specification is a value measured by gel permeation chromatography (GPC) in terms of standard polystyrene.
[0042] The adhesive may contain one or more types of energy ray-curable resins. When the adhesive contains two or more types of energy ray-curable resins, the combination and ratio thereof can be selected arbitrarily.
[0043] When an energy ray curable resin or a thermosetting resin is used, it is preferable to use a photopolymerization initiator, a thermal polymerization initiator, etc. By using a photopolymerization initiator, a thermal polymerization initiator, etc., the polymerization reaction of the curable resin can be easily initiated, and the curing reaction can be easily controlled.
[0044] Examples of the photopolymerization initiator include photoradical polymerization initiators such as benzophenone, acetophenone, benzoin, benzoin methyl ether, 2,4-diethylthioxanthone, 1-hydroxycyclohexyl phenyl ketone, benzyl diphenyl sulfide, tetramethylthiuram monosulfide, azobisisobutyronitrile, 2-chloroanthraquinone, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, and bis(2,4,6-trimethylbenzoyl)-phenyl-phosphine oxide.
[0045] In addition to photoradical polymerization initiators, photocationic polymerization initiators can also be used as photopolymerization initiators. A photocationic polymerization initiator is a compound that generates cationic species when irradiated with energy rays, thereby initiating the curing reaction of a cationic curable compound, and is composed of a cationic moiety that absorbs energy rays and an anionic moiety that serves as an acid generation source.
[0046] Examples of the photocationic polymerization initiator include sulfonium salt compounds, iodonium salt compounds, phosphonium salt compounds, ammonium salt compounds, antimonate compounds, diazonium salt compounds, selenium salt compounds, oxonium salt compounds, bromine salt compounds, etc. Among these, from the viewpoints of excellent compatibility and excellent storage stability of the resulting adhesive, sulfonium salt compounds are preferred, and aromatic sulfonium salt compounds having an aromatic group are more preferred.
[0047] Examples of sulfonium salt compounds include triphenylsulfonium hexafluorophosphate, triphenylsulfonium hexafluoroantimonate, and triphenylsulfonium tetrakis(pentafluorophenyl)borate.
[0048] Examples of iodonium salt compounds include diphenyliodonium tetrakis(pentafluorophenyl)borate, diphenyliodonium hexafluorophosphate, and (tricumyl)iodonium tetrakis(pentafluorophenyl)borate.
[0049] Examples of the phosphonium salt compounds include tri-n-butyl(2,5-dihydroxyphenyl)phosphonium bromide and hexadecyltributylphosphonium chloride.
[0050] Examples of the ammonium salt compound include benzyltrimethylammonium chloride, phenyltributylammonium chloride, and benzyltrimethylammonium bromide.
[0051] Examples of antimonate compounds include triphenylsulfonium hexafluoroantimonate, p-(phenylthio)phenyldiphenylsulfonium hexafluoroantimonate, and diaryliodonium hexafluoroantimonate.
[0052] Examples of the thermal polymerization initiator include thermal radical polymerization initiators such as hydrogen peroxide; peroxodisulfates such as ammonium peroxodisulfate, sodium peroxodisulfate, and potassium peroxodisulfate; azo compounds such as 2,2'-azobis(2-amidinopropane) dihydrochloride, 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobisisobutyronitrile, and 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile); and organic peroxides such as benzoyl peroxide, lauroyl peroxide, peracetic acid, persuccinic acid, di-t-butyl peroxide, t-butyl hydroperoxide, and cumene hydroperoxide.
[0053] In addition to the above-mentioned thermal radical polymerization initiators, examples of the thermal polymerization initiator include thermal cationic polymerization initiators. The thermal cationic polymerization initiator is a compound that can generate cationic species that initiate polymerization by heating. Examples of the thermal cationic polymerization initiator include sulfonium salts, quaternary ammonium salts, phosphonium salts, diazonium salts, and iodonium salts. Among these, sulfonium salts are preferred from the viewpoints of easy availability and the ease with which a product with superior adhesion and transparency can be obtained.
[0054] Examples of sulfonium salts include triphenylsulfonium tetrafluoroborate, triphenylsulfonium hexafluoroantimonate, and triphenylsulfonium hexafluoroarsinate.
[0055] Examples of quaternary ammonium salts include tetrabutylammonium tetrafluoroborate, tetrabutylammonium hexafluorophosphate, and tetrabutylammonium hydrogen sulfate. Examples of phosphonium salts include ethyltriphenylphosphonium hexafluoroantimonate and tetrabutylphosphonium hexafluoroantimonate.
[0056] Examples of diazonium salts include benzenediazonium chloride, etc. Examples of iodonium salts include diphenyliodonium hexafluoroarsinate, bis(4-chlorophenyl)iodonium hexafluoroarsinate, and phenyl(4-methoxyphenyl)iodonium hexafluoroarsinate, etc.
[0057] These polymerization initiators can be used alone or in combination of two or more. When these polymerization initiators are used to form a crosslinked structure, the amount used is preferably 0.1 parts by mass or more and 30 parts by mass or less, more preferably 0.5 parts by mass or more and 20 parts by mass or less, and particularly preferably 1 part by mass or more and 10 parts by mass or less, relative to 100 parts by mass of the energy ray-curable resin or the thermosetting resin.
[0058] When a thermosetting resin is used, a curing catalyst such as an imidazole-based curing catalyst may be used.
[0059] In this embodiment, the curable adhesive may contain a flexibility-adjusting component together with the energy ray-curable resin or the thermosetting resin to facilitate maintaining the sheet shape before curing. Examples of polymers used as the flexibility-adjusting component include phenoxy resin, polyolefin resin or modified polyolefin resin, polyamide-imide resin, polyimide resin, rubber-based resin, and acrylic resin.
[0060] These flexibility-adjusting components may be used alone or in combination of two or more.
[0061] When the curable adhesive used in this embodiment contains a flexibility-adjusting component, the total amount of the energy ray-curable resin and thermosetting resin contained in the adhesive is preferably 15 parts by mass or more and 300 parts by mass or less, more preferably 30 parts by mass or more and 250 parts by mass or less, and even more preferably 60 parts by mass or more and 200 parts by mass or less, per 100 parts by mass of the flexibility-adjusting component, from the viewpoint of adjusting the storage modulus of the first resin layer 4 within the above-mentioned range. Furthermore, when the adhesive contains an energy ray-curable resin or a thermosetting resin but does not contain a flexibility-adjusting component, the storage modulus of the first resin layer 4 tends to be too high.
[0062] In this embodiment, the curable adhesive preferably does not contain a filler. When the adhesive does not contain a filler, it is possible to prevent the storage modulus at 23°C of the first resin layer 4 from becoming too high. However, the curable adhesive may contain a filler to the extent that the storage modulus at 23°C of the first resin layer 4 can be adjusted to fall within the above range.
[0063] Examples of fillers include inorganic powders such as silica, alumina, talc, calcium carbonate, titanium white, red iron oxide, silicon carbide, and boron nitride; beads obtained by spheroidizing inorganic powders, single-crystal fibers, and glass fibers. Among these, silica filler and alumina filler are preferred. The fillers may be used alone or in combination of two or more.
[0064] The curable adhesive may contain other components, such as well-known additives, such as organic solvents, coupling agents, flame retardants, tackifiers, UV absorbers, antioxidants, preservatives, antifungal agents, plasticizers, antifoaming agents, and wettability adjusters.
[0065] (Electrode) The electrode 5 is used to supply current to the conductive linear body 31. The electrodes 5 form a pair. The electrode 5 is in direct contact with the conductive linear body 31. The electrode 5 is arranged so as to be electrically connected to both ends of the conductive linear body 31. The electrode 5 can be formed using a known electrode material. Examples of the electrode material include a conductive paste such as silver paste, a metal foil such as copper foil, and a metal wire. When the electrode material is a metal wire, the number of metal wires may be one, but preferably two or more.
[0066] When the electrode material is a metal foil or metal wire, examples of the metal of the metal foil or metal wire include copper, aluminum, tungsten, iron, molybdenum, nickel, titanium, silver, and gold, or alloys containing two or more metals such as stainless steel, carbon steel, brass, phosphor bronze, zirconium-copper alloy, beryllium copper, iron-nickel, nichrome, nickel-titanium, Kanthal, Hastelloy, and rhenium-tungsten. The metal foil or metal wire may also be plated with gold, tin, zinc, silver, nickel, chromium, nickel-chromium alloy, solder, or the like.
[0067] The width of at least one of the electrodes 5 is preferably 10 mm or less, more preferably 3 mm or less, in a plan view of the laminate 100. The width of this electrode is preferably 0.1 mm or more, more preferably 0.5 mm or more. When at least one of the electrodes is a metal wire, the width of the electrode is the diameter of the metal wire, and when two or more metal wires are used, the width of one electrode refers to the sum of the diameters of the metal wires.
[0068] The thickness of the electrode 5 is preferably 2 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more. The thickness of the electrode 5 is preferably 200 μm or less, more preferably 100 μm or less, even more preferably 50 μm or less, and particularly preferably 25 μm or less. If the thickness of the electrode 5 is within the above range, the electrical conductivity is high and the resistance is low, and the resistance value with the pseudo-sheet structure can be kept low. Furthermore, sufficient strength as an electrode can be obtained. Note that when the electrode is a metal wire, the thickness of the electrode is the diameter of the metal wire.
[0069] (Second Resin Layer) The second resin layer 6 is provided between the first substrate 1 or the second substrate 2 and the wiring sheet 10. The second resin layer 6 has a lower storage modulus than the first resin layer 4. This second resin layer 6 can prevent cracks from occurring in the second substrate 2. In this embodiment, the second substrate 2 and the wiring sheet 10 are laminated via the second resin layer 6. From the viewpoint of preventing cracks, the storage modulus of the second resin layer 6 at 23°C is set to 1.0 × 10 4 Pa or more, 3.0×10 5 From the same viewpoint, the storage modulus of the second resin layer 6 at 23° C. is preferably 4.0×10 Pa or less. 4 Pa or more, and more preferably 8.0 × 10 4 The storage modulus of the second resin layer 6 at 23° C. is more preferably 2.5×10 Pa or more. 5 Pa or less, and more preferably 2.0 × 10 5 From the same viewpoint, the storage modulus of the second resin layer 6 at 105° C. is more preferably 5.0×10 Pa or less. 3 Pa or more, and 4 The storage modulus of the second resin layer 6 at 105°C is more preferably 4.0 × 10 Pa or more. 4 Pa or less, and 4 It is more preferable that the storage modulus is not more than Pa. The storage modulus can be measured by the method described in the examples below.
[0070] The thickness of the second resin layer 6 is not particularly limited. The thickness of the second resin layer 6 is preferably 1 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more. The thickness of the second resin layer 6 is preferably 1000 μm or less, more preferably 500 μm or less, and even more preferably 300 μm or less.
[0071] The second resin layer 6 is preferably a pressure-sensitive adhesive layer as described below, from the viewpoint of excellent performance as a pressure-sensitive adhesive layer and of setting the storage modulus within the above range.
[0072] The adhesive layer can be composed of an adhesive obtained by crosslinking (thermally crosslinking) an adhesive composition (hereinafter sometimes referred to as "adhesive composition P") containing, for example, a (meth)acrylic acid ester polymer (A) and a crosslinking agent (B), or an energy ray-curable component (C), or both. It is preferable that this adhesive composition P further contains a photopolymerization initiator (D) if desired. Furthermore, in this specification, "(meth)acrylic acid" means both acrylic acid and methacrylic acid. The same applies to other similar terms. Furthermore, "polymer" also includes the concept of "copolymer."
[0073] When the adhesive composition P contains the energy ray-curable component (C), the adhesive layer obtained by crosslinking the adhesive composition P has not yet been cured by energy rays and has a relatively low storage modulus at the stage of an adhesive sheet, i.e., before being attached to an adherend. Therefore, the stress generated when the adhesive layer is attached to an adherend can be alleviated. As a result, even when the adhesive layer is attached to an adherend surface having irregularities, the adhesive layer easily conforms to the irregularities, preventing gaps, lifting, etc. near the irregularities, and exhibiting excellent adhesion to the adherend.
[0074] The (meth)acrylic acid ester polymer (A) preferably contains, as monomer units constituting this polymer, a (meth)acrylic acid alkyl ester and a monomer having a reactive functional group in the molecule (reactive functional group-containing monomer).
[0075] The (meth)acrylic acid ester polymer (A) can exhibit desirable adhesiveness by containing a (meth)acrylic acid alkyl ester as a monomer unit constituting the polymer. As the (meth)acrylic acid alkyl ester, a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 20 carbon atoms is preferred. The alkyl group may be linear or branched, or may have a cyclic structure.
[0076] Examples of (meth)acrylic acid alkyl esters having an alkyl group containing 1 to 20 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, myristyl (meth)acrylate, palmityl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, and adamantyl (meth)acrylate. These may be used alone or in combination of two or more.
[0077] Among these, the (meth)acrylic acid alkyl ester is preferably a (meth)acrylic acid alkyl ester having an alkyl group with a carbon number of 4 to 20. As the (meth)acrylic acid alkyl ester having an alkyl group with a carbon number of 4 to 20, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isobornyl (meth)acrylate, etc. are preferred, and from the viewpoint of obtaining excellent adhesiveness, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isobornyl (meth)acrylate, etc. are more preferred, and n-butyl acrylate, 2-ethylhexyl acrylate, isobornyl acrylate, etc. are particularly preferred.
[0078] The (meth)acrylic acid ester polymer (A) preferably contains 40% by mass or more, more preferably 50% by mass or more, even more preferably 60% by mass or more, and particularly preferably 70% by mass or more of (meth)acrylic acid alkyl ester as a monomer unit constituting this polymer. When the (meth)acrylic acid alkyl ester is contained in an amount of 40% by mass or more, the (meth)acrylic acid ester polymer (A) can exhibit suitable adhesiveness. Furthermore, the (meth)acrylic acid ester polymer (A) preferably contains 99% by mass or less of (meth)acrylic acid alkyl ester as a monomer unit constituting this polymer, particularly preferably 95% by mass or less, and even more preferably 90% by mass or less. By making the (meth)acrylic acid alkyl ester 99% by mass or less, other monomer components can be introduced into the (meth)acrylic acid ester polymer (A) in suitable amounts. In particular, when the (meth)acrylic acid ester polymer (A) contains a hydroxyl group-containing monomer as a monomer constituting this polymer, the (meth)acrylic acid ester polymer (A) preferably contains 87 mass% or less, and more preferably 83 mass% or less, of a (meth)acrylic acid alkyl ester as a monomer unit constituting this polymer.
[0079] The (meth)acrylic acid ester polymer (A) contains a reactive functional group-containing monomer as a monomer unit constituting this polymer, and thus reacts with the crosslinking agent (B) described below via the reactive functional group derived from the reactive functional group-containing monomer, thereby forming a crosslinked structure (three-dimensional network structure), and a pressure-sensitive adhesive having the desired cohesive strength is obtained.
[0080] Preferred examples of the reactive functional group-containing monomer contained in the (meth)acrylic acid ester polymer (A) as a monomer unit constituting this polymer include a monomer having a hydroxyl group in the molecule (hydroxyl group-containing monomer), a monomer having a carboxyl group in the molecule (carboxyl group-containing monomer), and a monomer having an amino group in the molecule (amino group-containing monomer), etc. These reactive functional group-containing monomers may be used alone or in combination of two or more.
[0081] Among the reactive functional group-containing monomers, hydroxyl group-containing monomers or carboxyl group-containing monomers are preferred from the viewpoint of ease of adjusting the crosslink density and of obtaining a pressure-sensitive adhesive having the desired cohesive strength, and hydroxyl group-containing monomers are preferred from the viewpoint of adhesive strength and resistance to wet heat whitening.
[0082] Examples of hydroxyl group-containing monomers include (meth)acrylic acid hydroxyalkyl esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. Among these, (meth)acrylic acid hydroxyalkyl esters having a hydroxyalkyl group having 1 to 4 carbon atoms are preferred. Specific examples include 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate, and particularly preferred are 2-hydroxyethyl acrylate and 4-hydroxybutyl acrylate. These may be used alone or in combination of two or more.
[0083] Examples of the carboxyl group-containing monomer include ethylenically unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, itaconic acid, and citraconic acid. Among these, acrylic acid is preferred from the viewpoint of the cohesive strength of the resulting (meth)acrylic acid ester polymer (A). These may be used alone or in combination of two or more.
[0084] The (meth)acrylic acid ester polymer (A) preferably contains 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more of a reactive functional group-containing monomer as a monomer unit constituting this polymer. When the reactive functional group-containing monomer is a hydroxyl group-containing monomer, it is preferably contained in an amount of 5% by mass or more, more preferably 8% by mass or more, and even more preferably 10% by mass or more. When the reactive functional group-containing monomer is a hydroxyl group-containing monomer, it is preferably contained in an amount of less than 25% by mass, more preferably 20% by mass or less, and even more preferably 16% by mass or less. Furthermore, the (meth)acrylic acid ester polymer (A) preferably contains 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less of a reactive functional group-containing monomer as a monomer unit constituting this polymer.
[0085] In addition, it is also preferable that the (meth)acrylic acid ester polymer (A) contains a nitrogen atom-containing monomer as a monomer unit constituting this polymer. By having the nitrogen atom-containing monomer present as a constituent unit in the polymer, a predetermined polarity is imparted to the pressure-sensitive adhesive, and it can be made to have excellent affinity even for adherends having a certain degree of polarity, such as glass. Examples of the nitrogen atom-containing monomer include, in addition to the amino group-containing monomer as the reactive functional group-containing monomer described above, a monomer having an amide group and a monomer having a nitrogen-containing heterocycle. Among these, a monomer having a nitrogen-containing heterocycle is preferred from the viewpoint of imparting appropriate rigidity to the (meth)acrylic acid ester polymer (A).
[0086] Examples of the nitrogen atom-containing monomer that can be used include N-vinylcarboxylic acid amide, (meth)acrylamide, N-methyl(meth)acrylamide, N-methylol(meth)acrylamide, N-tert-butyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-ethyl(meth)acrylamide, N,N-dimethylaminopropyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-phenyl(meth)acrylamide, dimethylaminopropyl(meth)acrylamide, and N-vinylcaprolactam. These nitrogen atom-containing monomers may be used alone or in combination of two or more.
[0087] Examples of monomers having a nitrogen-containing heterocycle include N-(meth)acryloylmorpholine, N-vinyl-2-pyrrolidone, N-(meth)acryloylpyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-(meth)acryloylaziridine, aziridinylethyl (meth)acrylate, 2-vinylpyridine, 4-vinylpyridine, 2-vinylpyrazine, 1-vinylimidazole, N-vinylcarbazole, and N-vinylphthalimide. Of these, N-(meth)acryloylmorpholine, which exhibits superior adhesive strength, is preferred, and N-acryloylmorpholine (4-acryloylmorpholine) is particularly preferred.
[0088] When the (meth)acrylic acid ester polymer (A) contains a monomer having a nitrogen-containing heterocycle as a monomer unit constituting this polymer, it preferably contains 0.5% by mass or more of the nitrogen atom-containing monomer, more preferably 1% by mass or more, and even more preferably 3% by mass or more. Furthermore, the (meth)acrylic acid ester polymer (A) preferably contains 20% by mass or less of the nitrogen-containing heterocycle as a monomer unit constituting this polymer, more preferably 15% by mass or less, and even more preferably 8% by mass or less. When the content of the monomer having a nitrogen-containing heterocycle is within the above range, the resulting pressure-sensitive adhesive can effectively exhibit excellent adhesion to adherends such as glass.
[0089] The (meth)acrylic acid ester polymer (A) may contain other monomers as monomer units constituting this polymer, if desired. Examples of other monomers include (meth)acrylic acid alkoxyalkyl esters such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate, vinyl acetate, and styrene. These may be used alone or in combination of two or more.
[0090] The (meth)acrylic acid ester polymer (A) is preferably a linear polymer. The linear polymer makes it easier for molecular chains to become entangled, which is expected to improve cohesive strength, thereby producing a superior pressure-sensitive adhesive.
[0091] The polymerization mode of the (meth)acrylic acid ester polymer (A) may be a random copolymer or a block copolymer.
[0092] The weight average molecular weight of the (meth)acrylic acid ester polymer (A) is preferably at least 200,000, more preferably at least 300,000, and even more preferably at least 400,000. When the lower limit of the weight average molecular weight of the (meth)acrylic acid ester polymer (A) is equal to or greater than the above limit, the second resin layer and the laminate have excellent long-term durability.
[0093] The weight average molecular weight of the (meth)acrylic acid ester polymer (A) is preferably 2,000,000 or less, more preferably 1,500,000 or less, even more preferably 1,000,000 or less, and particularly preferably 800,000 or less. When the upper limit of the weight average molecular weight of the (meth)acrylic acid ester polymer (A) is the above-mentioned or less, the resulting pressure-sensitive adhesive will have better at least one of the lamination property and adhesion to the adherend.
[0094] In the pressure-sensitive adhesive composition P, the (meth)acrylic acid ester polymer (A) may be used alone or in combination of two or more.
[0095] The crosslinking agent (B) crosslinks the (meth)acrylic acid ester polymer (A) by heating the pressure-sensitive adhesive composition P, thereby enabling the formation of a favorable three-dimensional network structure, thereby further improving the cohesive strength of the resulting pressure-sensitive adhesive.
[0096] The crosslinking agent (B) may be any that reacts with the reactive functional group of the (meth)acrylic acid ester polymer (A), such as isocyanate-based crosslinking agents, epoxy-based crosslinking agents, amine-based crosslinking agents, melamine-based crosslinking agents, aziridine-based crosslinking agents, hydrazine-based crosslinking agents, aldehyde-based crosslinking agents, oxazoline-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, and ammonium salt-based crosslinking agents. Among these, when the reactive functional group of the (meth)acrylic acid ester polymer (A) is a hydroxyl group, it is preferable to use an isocyanate-based crosslinking agent that has excellent reactivity with the hydroxyl group. When the reactive functional group of the (meth)acrylic acid ester polymer (A) is a carboxyl group, it is preferable to use an epoxy-based crosslinking agent that has excellent reactivity with the carboxyl group. The crosslinking agent (B) may be used alone or in combination of two or more.
[0097] The isocyanate-based crosslinking agent contains at least a polyisocyanate compound. Examples of polyisocyanate compounds include aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, and xylylene diisocyanate, aliphatic polyisocyanates such as hexamethylene diisocyanate, alicyclic polyisocyanates such as isophorone diisocyanate and hydrogenated diphenylmethane diisocyanate, and biuret and isocyanurate derivatives thereof, as well as adducts formed by reaction with low-molecular-weight active hydrogen-containing compounds such as ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, and castor oil. Among these, trimethylolpropane-modified aromatic polyisocyanates are preferred from the viewpoint of reactivity with hydroxyl groups, and it is particularly preferred to use at least one of trimethylolpropane-modified tolylene diisocyanate and trimethylolpropane-modified xylylene diisocyanate.
[0098] Examples of epoxy crosslinking agents include 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-m-xylylenediamine, ethylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane diglycidyl ether, diglycidylaniline, and diglycidylamine. Among these, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane is preferred from the viewpoint of reactivity with carboxy groups.
[0099] The content of the crosslinking agent (B) in the pressure-sensitive adhesive composition P is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). This content is preferably 3 parts by mass or less, more preferably 2 parts by mass or less, and even more preferably 1 part by mass or less. By having the content of the crosslinking agent (B) within the above range, the degree of crosslinking becomes appropriate, and the resulting pressure-sensitive adhesive becomes more excellent, as it becomes easier to adjust the storage modulus to a suitable value.
[0100] By including the energy ray-curable component (C) in the adhesive composition P, the adhesive obtained by crosslinking (thermal crosslinking) the adhesive composition P becomes an energy ray-curable adhesive. It is presumed that, when this adhesive is cured by energy ray irradiation after attachment to an adherend, the energy ray-curable components (C) polymerize with each other, and the polymerized energy ray-curable components (C) become entangled in the crosslinked structure (three-dimensional network structure) of the (meth)acrylic acid ester polymer (A). An adhesive having such a high-order structure has high cohesive strength and exhibits high coating strength.
[0101] The energy ray-curable component (C) is not particularly limited as long as it is a component that can be cured by irradiation with energy rays and can provide the above-mentioned effects, and may be any of a monomer, an oligomer, a polymer, or a mixture thereof. Among these, preferred is a polyfunctional acrylate-based monomer that has excellent compatibility with the (meth)acrylic acid ester polymer (A) and the like.
[0102] Examples of polyfunctional acrylate monomers include bifunctional monomers such as tricyclodecane dimethanol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, neopentyl glycol adipate di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, caprolactone-modified dicyclopentenyl di(meth)acrylate, ethylene oxide-modified phosphate di(meth)acrylate, di(acryloxyethyl)isocyanurate, allylated cyclohexyl di(meth)acrylate, ethoxylated bisphenol A diacrylate, and 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene. trifunctional types such as trimethylolpropane tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, propionic acid-modified dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide-modified trimethylolpropane tri(meth)acrylate, tris(acryloxyethyl)isocyanurate, and ε-caprolactone-modified tris-(2-(meth)acryloxyethyl)isocyanurate; tetrafunctional types such as diglycerin tetra(meth)acrylate and pentaerythritol tetra(meth)acrylate; pentafunctional types such as propionic acid-modified dipentaerythritol penta(meth)acrylate; and hexafunctional types such as dipentaerythritol hexa(meth)acrylate and caprolactone-modified dipentaerythritol hexa(meth)acrylate. Among the above, it is preferable to use at least one of ε-caprolactone-modified tris-(2-(meth)acryloxyethyl)isocyanurate and tricyclodecane dimethanol di(meth)acrylate. These may be used alone or in combination of two or more. Furthermore, from the viewpoint of compatibility with the (meth)acrylic acid ester polymer (A), it is preferable that the polyfunctional acrylate monomer has a molecular weight of less than 1,000.
[0103] The content of the energy ray-curable component (C) in the pressure-sensitive adhesive composition P is preferably 1 part by mass or more, more preferably 2 parts by mass or more, even more preferably 3 parts by mass or more, and particularly preferably 5 parts by mass or more, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A), from the viewpoint of easily adjusting the storage modulus of the resulting pressure-sensitive adhesive to the desired value. On the other hand, from the viewpoint of preventing phase separation of the energy ray-curable component (C) from the (meth)acrylic acid ester polymer (A) and easily adjusting the storage modulus to the desired value, this content is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, even more preferably 20 parts by mass or less, and particularly preferably 7.5 parts by mass or less.
[0104] When ultraviolet rays are used as the energy rays to cure the energy ray-curable pressure-sensitive adhesive, it is preferable that the pressure-sensitive adhesive composition P further contains a photopolymerization initiator (D). By containing the photopolymerization initiator (D) in this way, the energy ray-curable component (C) can be polymerized efficiently, and the polymerization and curing time and the energy ray irradiation dose can be reduced.
[0105] Examples of the photopolymerization initiator (D) include benzophenone, acetophenone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzoin benzoic acid, benzoin methyl benzoate, benzoin dimethyl ketal, 2,4-diethylthioxanthone, 1-hydroxycyclohexyl phenyl ketone, benzyl diphenyl sulfide, tetramethylthiuram monosulfide, azobisisobutyronitrile, benzyl, dibenzyl, diacetyl, β-chloroanthraquinone, 4-(2-hydroxyethoxy)-phenyl(2-hydroxy-2-propyl)ketone, 2-benzothiazole-N,N-diethyldithiocarbamate, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide. These may be used alone or in combination of two or more.
[0106] The content of the photopolymerization initiator (D) in the adhesive composition P is preferably 0.1 parts by mass or more, more preferably 1.0 parts by mass or more, and even more preferably 5.0 parts by mass or more, relative to 100 parts by mass of the energy ray-curable component (C). Furthermore, this content is preferably 35 parts by mass or less, more preferably 25 parts by mass or less, and even more preferably 15 parts by mass or less. When the content of the photopolymerization initiator (D) is within this range, it cleaves without any problems upon energy ray irradiation, further improving the curability of the energy ray-curable component (C). Furthermore, the storage modulus described above is more likely to be satisfied.
[0107] If desired, various additives commonly used in acrylic pressure-sensitive adhesives may be used in the pressure-sensitive adhesive composition P. Examples of the various additives include a silane coupling agent, an antistatic agent, a tackifier, an antioxidant, a light stabilizer, a softener, a filler, and a refractive index adjuster.
[0108] (Method for Manufacturing Laminate) There are no particular limitations on the method for manufacturing the laminate 100 according to this embodiment. The laminate 100 can be manufactured, for example, by the following steps. First, a step of manufacturing a wiring body film including the wiring body 3 is performed. In this step, a thermosetting adhesive for forming the first resin layer 4 is applied onto a release film to form a coating film. Next, the coating film is dried to form an adhesive layer. Next, the conductive linear bodies 31 are arranged and disposed on the adhesive layer to form the wiring body 3. For example, with the adhesive layer with a release film disposed on the outer circumferential surface of a drum member, the conductive linear bodies 31 are spirally wound around the adhesive layer while the drum member is rotated. Then, the bundle of spirally wound conductive linear bodies 31 is cut along the axial direction of the drum member. This forms the wiring body 3, which is then disposed on the adhesive layer. In this way, a wiring body film is obtained in which the wiring body 3 is formed on the adhesive layer with a release film. According to this method, for example, while rotating the drum member, the unreeled portion of the conductive linear member 31 is moved in a direction parallel to the axis of the drum member, thereby easily adjusting the distance L between adjacent conductive linear members 31 in the wiring body 3. Next, a step of providing a pair of electrodes 5 on the first substrate 1 is performed. In this step, the pair of electrodes 5 can be provided on the first substrate 1 by, for example, printing a conductive paste or the like in a predetermined arrangement and drying it. Next, a step of placing a wiring body film on the first substrate 1 on which the pair of electrodes 5 is provided and curing a thermosetting adhesive is performed. In this step, the wiring body film is bonded to the first substrate 1 on which the pair of electrodes 5 is provided so that the pair of electrodes 5 contact both ends of the conductive linear members 31 in the wiring body 3 of the wiring body film. Then, after peeling off the release film, a predetermined heat treatment is performed on the thermosetting adhesive to form a first resin layer 4, and a wiring sheet 10 is formed on the first substrate 1.
[0109] Meanwhile, a step of preparing a protective film including a second substrate 2 and a second resin layer 6 is performed. In this step, an adhesive composition P for forming the second resin layer 6 is applied to the second substrate 2 to form a coating film, thereby preparing the protective film. As shown in FIGS. 1 and 2 , it is preferable to provide two holes in the second substrate 2. Next, a step of placing the protective film on the first substrate 1 on which the wiring sheet 10 is provided and crosslinking the adhesive composition P is performed. In this step, the protective film is attached to the first substrate 1 on which the wiring sheet 10 is provided so that, in a plan view, the two holes in the protective film overlap the pair of electrodes 5 and the coating film of the adhesive composition P on the protective film contacts the wiring sheet 10. Then, the coating film of the adhesive composition P is irradiated with a predetermined energy ray to form the second resin layer 6, thereby preparing the laminate 100.
[0110] (Effects of First Embodiment) According to this embodiment, the following effects can be achieved. (1) According to this embodiment, the second resin layer 6 is easily deformed due to its low storage modulus. Therefore, when the laminate 100 reaches a high temperature, the second resin layer 6 deforms, thereby alleviating the strain occurring in the second substrate 2. In this way, it is possible to prevent cracks from occurring in the second substrate 2. (2) According to this embodiment, the storage modulus of the second resin layer 6 at 23°C can be increased to 1.0 x 10 4 Pa or more, 3.0×10 5 By setting the storage modulus of the first resin layer 4 at 23° C. to 5.0×10 or less, the second resin layer 6 can be easily deformed, and distortion occurring in the second base material 2 can be alleviated. (3) According to this embodiment, the first resin layer 4 can fix the conductive linear body 31, suppress deformation in the thickness direction inside the laminate 100, stabilize contact between the conductive linear body 31 and the electrode 5, and stabilize the resistance value of the wiring body 3. (4) According to this embodiment, the storage modulus of the first resin layer 4 at 23° C. can be set to 5.0×10 or less. 6 Pa or more, 1.0×10 10 By setting the stress to be equal to or less than Pa, when deformation is applied to the laminate 100, it is possible to fix the conductive linear body 31 while preventing the connection portion between the conductive linear body 31 and the electrode 5 from being broken. (5) The laminate 100 according to this embodiment can be produced by a relatively simple method using the above-described laminate production method.
[0111] [Second Embodiment] Next, a second embodiment of the present invention will be described with reference to the drawings. The present invention is not limited to the contents of this embodiment. In the drawings, some parts are illustrated enlarged or reduced to facilitate explanation. The second embodiment differs from the first embodiment in that, in a cross-sectional view of the laminate 100A, the first substrate 1 and the wiring sheet 10 are laminated via a second resin layer 6. In the following explanation, differences from the first embodiment will be mainly explained, and overlapping explanations will be omitted or simplified. Configurations similar to those in the first embodiment will be assigned the same reference numerals, and explanations will be omitted or simplified.
[0112] 3 , the laminate 100A according to this embodiment includes a first substrate 1, a second substrate 2 having a higher linear expansion coefficient than the first substrate 1, and a wiring sheet 10 sandwiched between the first substrate 1 and the second substrate 2. The wiring sheet 10 includes a wiring body 3 having a plurality of conductive linear bodies 31 arranged at intervals, a first resin layer 4 that directly or indirectly supports the wiring body 3, and a pair of electrodes 5 in direct contact with the conductive linear bodies 31. The first substrate 1 and the wiring sheet 10 are laminated together via a second resin layer 6 having a storage modulus lower than that of the first resin layer 4.
[0113] (Operations and Effects of Second Embodiment) According to this embodiment, the operations and effects (1) to (4) of the first embodiment can be achieved.
[0114] [Modifications of the Embodiments] The present invention is not limited to the above-described embodiments, and modifications or improvements within the scope of achieving the object of the present invention are included in the present invention. For example, in the above-described embodiment, the laminate 100 includes a film-like first substrate 1, but is not limited thereto. For example, the first substrate 1 may be a substrate formed into a three-dimensional shape. In such a case, the wiring sheet 10 can be attached to the first substrate 1, which is the adherend, by the first resin layer 4 or the second resin layer 6. In the second embodiment described above, the cross-sectional view of the laminate 100A shows that the first substrate 1 and the wiring sheet 10 are laminated via the second resin layer 6, but modifications are not limited thereto. For example, two other modifications can be mentioned. One modification is an example in which the wiring sheet 10 is reversed from the first embodiment (the electrode 5 is provided on the second substrate 2 side). Another modification is an example in which the wiring sheet 10 is reversed from the second embodiment (the electrode 5 is provided on the second substrate 2).
[0115] The present invention will be described in more detail below with reference to examples. The present invention is not limited to these examples. The laminates obtained in the examples were evaluated as follows.
[0116] [Evaluation of Cracks] The laminate was left standing at 105° C. for 1000 hours, and then the presence or absence of cracks in the base layer of the laminate was confirmed using a digital microscope.
[0117] [Storage Modulus Measurement] A cylindrical test sample with a diameter of 8 mm and a thickness of 1 mm was prepared from the same composition as the composition forming the layer to be measured. The storage modulus of the test sample was measured using a viscoelasticity measuring device (manufactured by Anton Paar, model name "MCR300") using parallel plates with a diameter of 8 mm as a measuring jig under the following conditions: test start temperature -20°C, test end temperature 150°C, heating rate 3°C / min, shear strain 0.05%, and frequency 1 Hz.
[0118] [Measurement of Linear Expansion Coefficient] The substrate was cut into a 4.5 mm × 20 mm rectangle to prepare a test sample. The linear expansion coefficient of the test sample was measured using a thermomechanical analyzer (manufactured by Netsch Japan, product name "TMA4000SE") under the conditions of a tensile load of 2 g, a temperature range of 23 to 105°C, and a heating rate of 5°C / min.
[0119] Preparation Example 1 A curable adhesive was obtained by blending 100 parts by mass of a phenoxy resin (manufactured by Mitsubishi Chemical Corporation, product name "YX7200B35") with 170 parts by mass of a polyfunctional hydrogenated bisphenol A diglycidyl ether epoxy compound (manufactured by Mitsubishi Chemical Corporation, product name "YX8000"), 0.2 parts by mass of a silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd., product name "KBM-4803"), 2 parts by mass of a thermal cationic polymerization initiator (manufactured by Sanshin Chemical Industry Co., Ltd., product name "SAN-AID SI-B3"), and 2 parts by mass of a thermal cationic polymerization initiator (manufactured by Sanshin Chemical Industry Co., Ltd., product name "SAN-AID SI-B7").
[0120] Preparation Example 2 (Preparation of (meth)acrylic acid ester polymer (A)) 65 parts by mass of 2-ethylhexyl acrylate, 5 parts by mass of 4-acryloylmorpholine, 15 parts by mass of isobornyl acrylate, and 15 parts by mass of 2-hydroxyethyl acrylate were copolymerized to prepare a (meth)acrylic acid ester polymer (A). When the molecular weight of this (meth)acrylic acid ester polymer (A) was measured, it was found to have a weight average molecular weight (Mw) of 500,000. In addition, the glass transition temperature (Tg, units: ° C) of this (meth)acrylic acid ester polymer (A) was calculated using the FOX formula based on the glass transition temperatures (Tg) of the respective monomers constituting the (meth)acrylic acid ester polymer (A) as homopolymers, and was found to be −36.5° C. (Preparation of adhesive composition) 100 parts by mass of the obtained (meth)acrylic acid ester polymer (A) (solid content equivalent value, the same applies hereinafter), 0.18 parts by mass of trimethylolpropane-modified tolylene diisocyanate as the crosslinking agent (B), 7 parts by mass of ε-caprolactone-modified tris-(2-acryloxyethyl)isocyanurate as the energy ray-curable component (C), 0.7 parts by mass of a mixture of benzophenone and 1-hydroxycyclohexyl phenyl ketone in a 1:1 mass ratio as the photopolymerization initiator (D), and 0.28 parts by mass of 3-glycidoxypropyltrimethoxysilane as the silane coupling agent were mixed, thoroughly stirred, and diluted with methyl ethyl ketone to obtain a coating solution of an adhesive composition.
[0121] [Preparation Example 3] (Preparation of adhesive composition) 100 parts by mass of the (meth)acrylic acid ester polymer (A) obtained in Preparation Example 2, 0.15 parts by mass of trimethylolpropane-modified tolylene diisocyanate as the crosslinking agent (B), 5 parts by mass of ε-caprolactone-modified tris-(2-acryloxyethyl)isocyanurate as the energy ray-curable component (C), 0.5 parts by mass of 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide as the photopolymerization initiator (D), and 0.25 parts by mass of 3-glycidoxypropyltrimethoxysilane as the silane coupling agent were mixed, thoroughly stirred, and diluted with methyl ethyl ketone to obtain a coating solution of an adhesive composition.
[0122] Preparation Example 4 (Preparation of (meth)acrylic acid ester polymer (A)) 30 parts by mass of 2-ethylhexyl acrylate, 25 parts by mass of n-butyl acrylate, 5 parts by mass of 4-acryloylmorpholine, 15 parts by mass of isobornyl acrylate, and 25 parts by mass of 2-hydroxyethyl acrylate were copolymerized to prepare a (meth)acrylic acid ester polymer (A). When the molecular weight of this (meth)acrylic acid ester polymer (A) was measured, it was found to have a weight average molecular weight (Mw) of 600,000. (Preparation of adhesive composition) 100 parts by mass of the obtained (meth)acrylic acid ester polymer (A), 0.2 parts by mass of trimethylolpropane-modified tolylene diisocyanate as a crosslinking agent (B), 8.0 parts by mass of ε-caprolactone-modified tris-(2-acryloxyethyl)isocyanurate as an energy ray-curable component (C), 0.8 parts by mass of 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide as a photopolymerization initiator (D), and 0.2 parts by mass of 3-glycidoxypropyltrimethoxysilane as a silane coupling agent were mixed, thoroughly stirred, and diluted with methyl ethyl ketone to obtain a coating solution of an adhesive composition.
[0123] Example 1 (Preparation of Wiring Film) The curable adhesive obtained in Preparation Example 1 was applied to a 38 μm-thick release film (manufactured by Lintec Corporation, product name "SP-382150") to a thickness of 15 μm, and the film was cut into a 250 mm x 320 mm rectangle to prepare an adhesive sheet. A gold-plated tungsten wire (10 μm diameter, hereinafter also referred to as "wire") was prepared as the conductive linear body. Next, the resulting adhesive sheet was wrapped around a drum member with a rubber outer periphery, with the surface of the pressure-sensitive adhesive layer facing outward and free of wrinkles, and both ends of the adhesive sheet in the circumferential direction were fixed with double-sided tape. The wire wound around the bobbin was attached to the surface of the pressure-sensitive adhesive layer of the adhesive sheet located near the end of the drum member, and the wire was then unwound and wound around the drum member. The drum member was then gradually moved in a direction parallel to the drum axis so that the wire was wound around the drum member in a spiral at equal intervals of 3 mm. This resulted in a wiring body with 96 wires arranged on the surface of the adhesive. The wires were then cut, and the wiring body was removed from the drum member. The wiring body was cut into a 40 x 82 mm width so that 12 wires could be removed, and a wiring body film was produced.
[0124] (Preparation of Substrate with Electrode) A 2 mm thick glass substrate (linear expansion coefficient 3.3 × 10) was used as the first substrate. -6 Silver paste was screen-printed onto the substrate (at 150°C / °F) so as to have a width of 2 mm and an inter-electrode distance of 7.8 mm, and then dried at 150°C for 30 minutes to form strip electrodes with a thickness of 17 μm. The strip electrodes were then subjected to electroless plating to produce a substrate with electrodes.
[0125] (Formation of wiring sheet) The obtained wiring film was attached to the obtained electrode-attached substrate so that the electrodes were located at both ends of the wires. Thereafter, the substrate was heated at a temperature of 120°C and a pressure of 0.5 MPa for 30 minutes to harden the adhesive and form a first resin layer, thereby forming a wiring sheet on the first substrate. The storage modulus of the first resin layer at 23°C was 2.2 × 10 9 Pa, and the storage modulus of the first resin layer at 105°C is 1.6 × 10 9 It was Pa.
[0126] (Preparation of Protective Sheet) The adhesive composition solution obtained in Preparation Example 2 was applied to a thickness of 100 μm on a 100 μm thick cycloolefin polymer film (manufactured by Zeon Corporation, product name "ZF16") as a second substrate, and cut into a 50 mm × 120 mm rectangle. Then, a 5 mm diameter circle was cut out so that the center-to-center distance between the two circles was 7.8 mm, forming two holes to prepare a protective sheet. The linear expansion coefficient of the second substrate is shown in Table 1.
[0127] (Preparation of Laminate) A protective sheet was attached to the first substrate on which the wiring sheet was provided so that the electrodes of the wiring sheet and the circles of the protective sheet were aligned. Thereafter, ultraviolet light having a wavelength of 365 nm was applied at an illuminance of 200 mW / cm. 2 , light intensity 1000mJ / cm 2 The laminate was then irradiated under the conditions of (a) to (c) to form a second resin layer, thereby obtaining a laminate. The laminate was evaluated for cracks. The storage moduli of the second resin layer at 23°C and 105°C are shown in Table 1.
[0128] [Example 2] A laminate was produced in the same manner as in Example 1, except that the cycloolefin polymer film (manufactured by Zeon Corporation, product name "ZF16") of the protective sheet was changed to a polycarbonate film (manufactured by Teijin Limited, product name "L-100").
[0129] [Example 3] A laminate was produced in the same manner as in Example 1, except that the coating solution of the pressure-sensitive adhesive composition obtained in Protective Sheet Preparation Example 2 was changed to the coating solution of the pressure-sensitive adhesive composition obtained in Preparation Example 3.
[0130] [Comparative Example 1] A laminate was produced in the same manner as in Example 1, except that the coating solution of the pressure-sensitive adhesive composition obtained in Protective Sheet Preparation Example 2 was changed to the coating solution of the pressure-sensitive adhesive composition obtained in Preparation Example 4.
[0131] Comparative Example 2 A laminate was produced in the same manner as in Example 1, except that the coating solution of the pressure-sensitive adhesive composition obtained in Protective Sheet Preparation Example 2 was changed to the coating solution of the pressure-sensitive adhesive composition obtained in Preparation Example 4, and the cycloolefin polymer film (manufactured by Zeon Corporation, product name "ZF16") was changed to a polycarbonate film (manufactured by Teijin Limited, product name "L-100").
[0132]
[0133] As shown in Table 1, the laminates obtained in Examples 1 to 3 had good results in the crack evaluation. This confirmed that the present invention can provide a laminate that can prevent cracks from occurring in the substrate.
[0134] 1...first substrate, 2...second substrate, 3...wiring body, 31...conductive linear body, 4...first resin layer, 5...electrode, 6...second resin layer, 10...wiring sheet, 100, 100A...laminate
Claims
1. A laminate comprising a first substrate, a second substrate having a linear expansion coefficient higher than that of the first substrate, and a wiring sheet sandwiched between the first substrate and the second substrate, wherein the wiring sheet comprises a wiring body having a plurality of conductive linear members arranged at intervals, a first resin layer supporting the wiring body directly or indirectly, and a pair of electrodes in direct contact with the conductive linear members, and wherein the first substrate or the second substrate and the wiring sheet are laminated via a second resin layer having a storage modulus lower than that of the first resin layer.
2. The laminate according to claim 1, wherein the storage modulus of the second resin layer at 23°C is 1.0 x 10 4 Pa or more, 3.0×10 5 The laminate has a modulus of elasticity of 10 Pa or less.
3. The laminate according to claim 1 or 2, wherein the storage modulus of the first resin layer at 23° C. is 5.0×10 6 Pa or more, 1.0×10 10 The laminate has a modulus of elasticity of 10 Pa or less.
4. The laminate according to claim 1 or 2, wherein the linear expansion coefficient of the first substrate is 0.01×10 -6 / ℃ or more, 10 x 10 -6 / °C or less.
5. The laminate according to claim 1 or 2, wherein the linear expansion coefficient of the second substrate is 50×10 -6 / ℃ or more, 100 x 10 -6 / °C or less.
6. A laminate according to claim 1 or 2, wherein the second base material and the wiring sheet are laminated via the second resin layer.
Citation Information
Patent Citations
Wiring sheet
WO2021225142A1
Heat fixing device
JP1979115252A
ceramic heater
JP1993011386U
Planar heater, its manufacturing method, and image fixing device
JP2006294604A
Substrate fixing device and manufacturing method of the same
JP2018026427A