Semiconductor device and method for manufacturing semiconductor device

The semiconductor device addresses parasitic resistance and carrier concentration issues by using a specific layer structure and manufacturing method, resulting in improved drain current and reduced leakage current in group III nitride semiconductor devices with two-dimensional electron gas channels.

WO2024204537A1PCT designated stage expired Publication Date: 2024-10-03NUVOTON TECH CORP JAPAN
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012641
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Group III nitride semiconductor devices with two-dimensional electron gas channels face issues with parasitic resistance and carrier concentration decrease due to crystal defects and contaminants when forming through recesses in the electron supply layer, leading to reduced maximum drain current.

Method used

A semiconductor device with an electron transit layer, an electron supply layer of larger band gap, and contact layers embedded in recesses, along with an n-type semiconductor layer and alloy layer, is manufactured using a method that forms insulating layers without atmospheric exposure, thinning, and heat treatment to reduce parasitic resistance and maintain electron concentration.

Benefits of technology

The solution effectively suppresses the decrease in maximum drain current and reduces leakage current by maintaining high electron concentration and minimizing crystal defects, enhancing the performance of group III nitride semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012641_03102024_PF_FP_ABST
    Figure JP2024012641_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A semiconductor device (1) having: an electron travel layer (103); an electron supply layer (104) that is provided on the electron-traveling layer (103); a gate electrode (303) that is provided on the electron-supply layer (104); a contact layer (212) that, at a position where the gate electrode (303) is enclosed on either side, is embedded in a through-recess part (211) passing through the electron supply layer (104); an electron supply auxiliary layer (401) that is provided so as to be in contact with the electron supply layer (104) and the contact layer (212) but not be in contact with the gate electrode (303), the electron supply auxiliary layer (401) being an example of a n-type semiconductor layer composed of a n-type semiconductor that contains Si; an alloy layer (402) that is provided on the electron supply auxiliary layer (401) and that contains Si; a first insulating layer (201) that is provided so as to be in contact with the gate electrode (303) but not be in contact with the contact layer (212); and a source electrode (301) and / or a drain electrode (302) that is provided on the contact layer (212) and the alloy layer (402).
Need to check novelty before this filing date? Find Prior Art

Description

Semiconductor device and manufacturing method thereof

[0001] The present disclosure relates to a semiconductor device and a manufacturing method thereof, and more particularly to a Group III nitride semiconductor device using a Group III nitride semiconductor and a manufacturing method thereof.

[0002] Group III nitride semiconductors, particularly those using gallium nitride (GaN) or aluminum gallium nitride (AlGaN), have high breakdown voltages due to the wide band gaps of the materials. Furthermore, heterostructures such as AlGaN / GaN can be easily formed in Group III nitride semiconductor devices.

[0003] In an AlGaN / GaN heterostructure, the difference between the piezoelectric polarization caused by the difference in lattice constant between the materials and the spontaneous polarization of AlGaN and GaN generates a high concentration of electrons (two-dimensional electron gas) on the GaN layer side of the interface between the AlGaN layer and the GaN layer, forming a channel of the two-dimensional electron gas layer. Group III nitride semiconductor devices that utilize this two-dimensional electron gas channel have a relatively high electron saturation velocity, relatively high insulation resistance, and relatively high thermal conductivity, and are therefore applied to high-frequency power devices, etc.

[0004] In order to improve the characteristics of these Group III nitride semiconductor devices, it is advisable to reduce as much as possible parasitic resistance components such as the contact between the ohmic electrode and the two-dimensional electron gas layer in the Group III nitride semiconductor device (hereinafter referred to as "ohmic contact") and the channel resistance due to the two-dimensional electron gas.

[0005] Conventionally, techniques for reducing ohmic contact resistance have been proposed for Group III nitride semiconductor devices that utilize a channel formed by two-dimensional electron gas. For example, Patent Document 1 discloses a technique for forming an ohmic electrode by forming a recess (hereinafter referred to as a "through recess") that penetrates an electron supply layer made of AlGaN in a portion of a Group III nitride semiconductor device where an ohmic electrode is to be formed, in order to reduce the ohmic contact resistance.

[0006] International Publication No. 2021 / 246227

[0007] However, when a through recess is formed in the electron supply layer as in the technology disclosed in Patent Document 1, it is inevitable that the two-dimensional electron gas layer and the contact layer embedded in the through recess will essentially be connected at a point. Furthermore, when a through recess is formed in the electron supply layer, not only do crystal defects occur at the interface between the two-dimensional electron gas layer (channel layer) made of GaN and the contact layer when the through recess is formed, but also atmospheric pollutants and bond defects cause a region of reduced carrier (electron) concentration in the electron supply layer adjacent to the side surface of the through recess, resulting in a decrease in the maximum drain current.

[0008] The present disclosure has been made in view of the above-described problems, and aims to provide a semiconductor device capable of suppressing a decrease in maximum drain current, and a method for manufacturing the same.

[0009] In order to achieve the above object, one aspect of the semiconductor device according to the present disclosure includes an electron transit layer, an electron supply layer provided on the electron transit layer and having a band gap larger than that of the electron transit layer, a gate electrode provided on the electron supply layer, source-side contact layers and drain-side contact layers embedded in recesses that penetrate the electron supply layer at positions on either side of the gate electrode, an n-type semiconductor layer made of an n-type semiconductor containing Si, provided in contact with the electron supply layer and in contact with the source-side contact layer and / or the drain-side contact layer but without in contact with the gate electrode, an alloy layer containing Si and having a thickness of 2 nm or less provided on the n-type semiconductor layer, an insulating layer provided on a portion of the electron supply layer where the gate electrode is not provided, in contact with the gate electrode but without in contact with the source-side contact layer and / or the drain-side contact layer, and a source electrode and / or a drain electrode provided on the source-side contact layer and / or the drain-side contact layer and on the alloy layer.

[0010] a step of forming a through-recess portion that penetrates the thin portion of the insulating layer and the electron supply layer to reach the electron transit layer while leaving a portion of the thin portion as a remaining insulating layer; a step of embedding a contact layer in the through-recess portion; a step of forming a source electrode and / or a drain electrode across the remaining insulating layer and the contact layer; a step of forming an alloy layer and an electron supply auxiliary layer in the remaining insulating layer and the electron supply layer by heat treatment; and a step of removing the insulating layer from a portion of the insulating layer that is spaced from the source electrode and / or the drain electrode to form a gate electrode.

[0011] a step of forming a through-recess portion that extends through the thin portion of the insulating layer and the electron supply layer to reach the electron transit layer while leaving a portion of the thin portion as a remaining insulating layer; a step of forming a source electrode and / or a drain electrode across the remaining insulating layer and the through-recess portion; a step of forming an alloy layer and an electron supply auxiliary layer in the remaining insulating layer and the electron supply layer by heat treatment; and a step of forming a gate electrode by removing a portion of the insulating layer that is spaced apart from the source electrode and / or the drain electrode.

[0012] According to the present disclosure, a semiconductor device capable of suppressing a decrease in maximum drain current can be obtained.

[0013] FIG. 1 is a cross-sectional view showing the configuration of a semiconductor device according to a first embodiment. FIG. 2 is a schematic diagram showing the conduction band of the energy band of the semiconductor device according to the first embodiment. FIG. 3A is a cross-sectional view showing a step of forming a semiconductor stacked structure and a first insulating layer and a second insulating layer in the method for manufacturing a semiconductor device according to the first embodiment. FIG. 3B is a cross-sectional view showing a step of forming a thin portion in the first insulating layer in the method for manufacturing a semiconductor device according to the first embodiment. FIG. 3C is a cross-sectional view showing a step of forming a through-hole recess in the method for manufacturing a semiconductor device according to the first embodiment. FIG. 3D is a cross-sectional view showing a step of forming a contact layer in the method for manufacturing a semiconductor device according to the first embodiment. FIG. 3E is a cross-sectional view showing a step of forming a source electrode and a drain electrode in the method for manufacturing a semiconductor device according to the first embodiment. FIG. 3F is a cross-sectional view showing a heat treatment step in the method for manufacturing a semiconductor device according to the first embodiment. FIG. 3G is a cross-sectional view showing a step of forming a gate electrode in the method for manufacturing a semiconductor device according to the first embodiment. FIG. 4 is a cross-sectional view showing the configuration of a semiconductor device according to a second embodiment. FIG. 5A is a cross-sectional view showing a step of forming a semiconductor stacked structure and a first insulating layer and a second insulating layer in the method for manufacturing a semiconductor device according to the second embodiment. Fig. 5B is a cross-sectional view showing a step of forming a thin portion in the first insulating layer in the method for manufacturing a semiconductor device according to the second embodiment. Fig. 5C is a cross-sectional view showing a step of forming a through recess portion in the method for manufacturing a semiconductor device according to the second embodiment. Fig. 5D is a cross-sectional view showing a step of forming a source electrode and a drain electrode in the method for manufacturing a semiconductor device according to the second embodiment. Fig. 5E is a cross-sectional view showing a step of performing a heat treatment in the method for manufacturing a semiconductor device according to the second embodiment. Fig. 5F is a cross-sectional view showing a step of forming a gate electrode in the method for manufacturing a semiconductor device according to the second embodiment.

[0014] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. Each embodiment shown here represents a specific example of the present disclosure. Therefore, the numerical values, shapes, components, arrangement and connection of the components, steps (processes), and order of steps shown in the following embodiments are merely examples and are not intended to limit the present disclosure. Therefore, among the components in the following embodiments, components that are not described in the independent claims that represent the superordinate concept of the present disclosure will be described as optional components.

[0015] Furthermore, each figure is a schematic diagram and is not necessarily an exact illustration. Therefore, the scales and the like do not necessarily match in each figure. In each figure, the same reference numerals are used to denote substantially the same components, and redundant explanations will be omitted or simplified.

[0016] Furthermore, in this specification, the terms "above," "upper," "below," and "belower" in the configuration of a semiconductor device do not refer to the upward direction (vertically upward) and downward direction (vertically downward) in absolute spatial recognition, but are terms defined by a relative positional relationship based on the stacking order in a stacked structure. Furthermore, the terms "above" and "below" are applied not only to a case where two components are arranged with a gap between them and another component exists between the two components, but also to a case where two components are arranged closely together and the two components are in contact with each other.

[0017] In addition, in this specification and the drawings, the x-axis, y-axis, and z-axis represent the three axes of a three-dimensional Cartesian coordinate system. In each embodiment, the two axes parallel to the top surface of the substrate of the semiconductor device are defined as the x-axis and y-axis, and the direction perpendicular to this top surface is defined as the z-axis direction. In the embodiments described below, the positive direction of the z-axis may be referred to as "up" and the negative direction of the z-axis may be referred to as "down." Note that in this specification, "planar view" refers to the substrate of the semiconductor device viewed from the positive direction of the z-axis.

[0018] First Embodiment First, a semiconductor device 1 according to a first embodiment will be described with reference to Fig. 1. Fig. 1 is a cross-sectional view showing the configuration of the semiconductor device 1 according to the first embodiment.

[0019] In this embodiment, a case will be described in which the semiconductor device 1 is a high electron mobility transistor (HEMT) having a Schottky junction gate structure.

[0020] As shown in FIG. 1, the semiconductor device 1 includes a substrate 101, a buffer layer 102, an electron transit layer 103, an electron supply layer 104, a first insulating layer 201, a second insulating layer 202, a source electrode 301, a drain electrode 302, a gate electrode 303, an electron supply assistance layer 401, and an alloy layer 402.

[0021] The substrate 101 is, for example, a silicon substrate made of Si. In this embodiment, the substrate 101 is, for example, a silicon substrate made of single-crystal Si with a (111) plane as the main surface. The substrate 101 is not limited to a silicon substrate, and may be a substrate made of sapphire, SiC, GaN, AlN, or the like, which serves as a base for forming a nitride semiconductor layer. The resistivity of the substrate 101 is, for example, 1 kΩ or more. The substrate 101 may have a resistivity of 20 Ω or less.

[0022] The buffer layer 102 is provided on the substrate 101. The buffer layer 102 is, for example, a 2 μm-thick Group III nitride semiconductor layer made of a multi-layer structure of AlN and AlGaN. In this case, 20 to 100 pairs of AlN and AlGaN may be stacked. 1-α Ga α The buffer layer 102 may have a structure in which multiple N (0≦α<0.8) layers are stacked, and may include a superlattice structure. Alternatively, the buffer layer 102 may be composed of a single layer or multiple layers of a group III nitride semiconductor such as InGaN or AlInGaN. The carbon concentration of the buffer layer 102 may be 1×10 19 atoms / cm 3 As described above, the resistance of the buffer layer 102 may be increased.

[0023] The electron transit layer 103 is provided on the buffer layer 102. In this embodiment, the electron transit layer 103 is, for example, a GaN layer made of GaN with a thickness of 150 nm. The Group III nitride semiconductor making up the electron transit layer 103 is not limited to GaN. The electron transit layer 103 may be made of a Group III nitride semiconductor such as InGaN, AlGaN, or AlInGaN. The electron transit layer 103 may also contain n-type impurities.

[0024] The electron supply layer 104 is provided on the electron transit layer 103. The electron supply layer 104 has a larger band gap than the electron transit layer 103. In this embodiment, the electron supply layer 104 is, for example, an AlGaN layer with a thickness of 13 nm and made of AlGaN with an Al composition ratio of 30%. A high concentration of two-dimensional electron gas is generated on the electron transit layer 103 side of the heterointerface between the electron supply layer 104 and the electron transit layer 103, forming a channel of the two-dimensional electron gas layer 105. Therefore, the semiconductor device 1 has the two-dimensional electron gas layer 105. As will be described in detail later, the two-dimensional electron gas layer 105 is composed of a first two-dimensional electron gas layer 105A and a second two-dimensional electron gas layer 105B having different electron concentrations of the two-dimensional electron gas.

[0025] The Al composition ratio of the electron supply layer 104 made of AlGaN is not limited to 30%. The Al composition ratio of the electron supply layer 104 may be 20 to 100%. Furthermore, the group III nitride semiconductor constituting the electron supply layer 104 is not limited to AlGaN. The electron supply layer 104 may be composed of a group III nitride semiconductor containing In, such as AlInGaN. Furthermore, the electron supply layer 104 may contain n-type impurities.

[0026] A cap layer may be provided on the electron supply layer 104. The cap layer may be, for example, a GaN layer made of GaN and having a thickness of about 1 to 2 nm. A spacer layer may be provided between the electron transit layer 103 and the electron supply layer 104. The spacer layer may be, for example, an AlN layer made of AlN and having a thickness of about 1 nm.

[0027] The first insulating layer 201 is provided on the electron supply layer 104. The first insulating layer 201 is an insulating layer containing Si (silicon). In this embodiment, the first insulating layer 201 is a SiN layer made of SiN. Specifically, the first insulating layer 201 is a SiN layer made of in-situ SiN and having a thickness of 2 nm. Note that "in-situ" means that it was formed without exposure to the atmosphere. Therefore, the first insulating layer 201 made of in-situ SiN is a SiN layer formed without exposure to the atmosphere after the electron supply layer 104 is formed.

[0028] By forming the first insulating layer 201 from in-situ SiN in this way, it is possible to eliminate uneven distribution of oxygen at the interface between the first insulating layer 201 and the electron supply layer 104. Eliminating uneven distribution of oxygen at the interface between the first insulating layer 201 and the electron supply layer 104 suppresses the generation of interface states. This makes it possible to avoid an increase in the potential at the interface and suppress a decrease in the electron concentration of the two-dimensional electron gas.

[0029] The thickness of the first insulating layer 201 is preferably 2 nm or more and 30 nm or less. By making the thickness of the first insulating layer 201 2 nm or more, it is possible to suppress uneven distribution of oxygen at the interface between the first insulating layer 201 and the electron supply layer 104 due to natural oxidation. On the other hand, if the thickness of the first insulating layer 201 exceeds 30 nm, the wafer will warp when the semiconductor device 1 is fabricated, degrading the quality of the semiconductor device 1. For this reason, it is preferable that the thickness of the first insulating layer 201 be 30 nm or less. In other words, by making the thickness of the first insulating layer 201 30 nm or less, it is possible to suppress warping of the wafer.

[0030] It is also preferable that the first insulating layer 201 does not contain oxygen. If the first insulating layer 201 contains oxygen, the interface state at the interface between the first insulating layer 201 and the electron supply layer 104 increases, the potential at the interface between the first insulating layer 201 and the electron supply layer 104 increases, and the electron concentration of the two-dimensional electron gas decreases. If the first insulating layer 201 does not contain oxygen, it is possible to suppress a decrease in the electron concentration of the two-dimensional electron gas.

[0031] The second insulating layer 202 is provided on the first insulating layer 201. In this embodiment, the second insulating layer 202 is in contact with the first insulating layer 201. The thickness of the second insulating layer 202 is thicker than the thickness of the first insulating layer 201, but is not limited to this. In other words, the thickness of the second insulating layer 202 may be thinner than the thickness of the first insulating layer 201. The second insulating layer 202 is made of, for example, SiO 2 The second insulating layer 202 is a silicon oxide layer having a thickness of 50 nm and is made of SiO 2 The material is not limited to this, and may be SiN, SiON, or the like.

[0032] An opening 201a is provided in the first insulating layer 201. The opening 201a is formed in a region of the first insulating layer 201 where the gate electrode 303 is to be provided. Therefore, the first insulating layer 201 is provided on a portion of the electron supply layer 104 where the gate electrode 303 is not provided.

[0033] An opening 202a is provided in the second insulating layer 202. The opening 202a is formed in the second insulating layer 202 in a region where the gate electrode 303 is to be provided. Therefore, the second insulating layer 202 is provided on a portion of the first insulating layer 201 where the gate electrode 303 is not provided.

[0034] The first insulating layer 201 and the second insulating layer 202 are in contact with the gate electrode 303. Furthermore, the first insulating layer 201 and the second insulating layer 202 are not in contact with the contact layer 212. In the present embodiment, the first insulating layer 201 and the second insulating layer 202 are not in contact with either the source-side contact layer 212A or the drain-side contact layer 212B, but this is not limiting. For example, the first insulating layer 201 may not be in contact with either the source-side contact layer 212A or the drain-side contact layer 212B, but may be in contact with the other. Furthermore, the second insulating layer 202 may not be in contact with either the source-side contact layer 212A or the drain-side contact layer 212B, but may be in contact with the other.

[0035] The electron supply layer 104 has a through-hole recess 211. In the present embodiment, the through-hole recess 211 is provided so as to penetrate through the first insulating layer 201 and the electron supply layer 104 and reach the electron transit layer 103. The through-hole recess 211 reaches the inside of the electron transit layer 103, and a recess is provided in the electron transit layer 103.

[0036] The distance from the upper surface of the electron transit layer 103 to the lowest part of the bottom surface of the through-hole recess 211 is preferably 10 nm or less. As an example, the distance from the upper surface of the electron transit layer 103 to the lowest part of the bottom surface of the through-hole recess 211 is 5 nm. The angle of elevation from the center to the side of the bottom surface of the through-hole recess 211 is preferably 10 degrees or less, and more preferably 5 degrees or less. This can reduce the occurrence of crystal defects on the side surface of the through-hole recess 211 when forming the through-hole recess 211 by dry etching, and can suppress a decrease in the maximum drain current.

[0037] The through-hole recess 211 is provided in a region corresponding to the region where the source electrode 301 and the drain electrode 302 are provided. Specifically, a pair of through-hole recesses 211 are provided so as to face each other with the gate electrode 303 interposed therebetween.

[0038] A contact layer 212 is provided in the through-hole recess 211. The contact layer 212 is provided so as to fill the through-hole recess 211. The contact layer 212 provided in one of the pair of through-hole recesses 211 is a source-side contact layer 212A, and the contact layer 212 provided in the other of the pair of through-hole recesses 211 is a drain-side contact layer 212B. The source-side contact layer 212A and the drain-side contact layer 212B are provided at positions sandwiching the gate electrode 303.

[0039] The through-hole recess 211 is provided at a distance from the first insulating layer 201 and the second insulating layer 202. Therefore, the contact layer 212 embedded in the through-hole recess 211 is also at a distance from the first insulating layer 201 and the second insulating layer 202, and the contact layer 212 is not in contact with the first insulating layer 201 or the second insulating layer 202.

[0040] The contact layer 212 is, for example, an n-GaN layer made of n-type GaN. The material making up the contact layer 212 is not limited to n-type GaN, and it may be made of a group III nitride semiconductor such as InGaN, AlGaN, or AlInGaN containing donors such as Si or Ge as n-type impurities, or may be made of a multilayer electrode film having a stacked structure in which Ti and Al are stacked in this order. The material making up the contact layer 212 may also be made of Ti, Ta, Al, Au, Hf, Ru, and Cu.

[0041] A source electrode 301 or a drain electrode 302 is provided on the contact layer 212. Specifically, the source electrode 301 is provided on the source-side contact layer 212A, and the drain electrode 302 is provided on the drain-side contact layer 212B. The source electrode 301 and the drain electrode 302 are provided to face each other with the gate electrode 303 interposed therebetween.

[0042] The source electrode 301 and the drain electrode 302 are provided on the contact layer 212 and the alloy layer 402. In this embodiment, the source electrode 301 and the drain electrode 302 also cover a portion of the second insulating layer 202. Specifically, the source electrode 301 is provided so as to cover the source-side contact layer 212A, the alloy layer 402, and a portion of the second insulating layer 202. The drain electrode 302 is provided so as to cover the drain-side contact layer 212B, the alloy layer 402, and a portion of the second insulating layer 202.

[0043] The source electrode 301 and the drain electrode 302 are formed of, for example, a multilayer electrode film having a laminate structure in which a 30 nm thick Ti film and a 200 nm thick Al film are laminated in this order, but are not limited to this. The source electrode 301 and the drain electrode 302 may also be formed using Ti, Ta, W, Al, Au, Hf, Ru, or Cu.

[0044] The gate electrode 303 is provided on the electron supply layer 104. Specifically, the gate electrode 303 is provided on the electron supply layer 104 via an opening 201a provided in the first insulating layer 201 and an opening 202a provided in the second insulating layer 202. Note that the opening width of the opening 201a in the first insulating layer 201 and the opening width of the opening 202a in the second insulating layer 202 are the same, but this is not limitative.

[0045] The gate electrode 303 is a multilayer electrode film having a laminated structure in which, for example, a TiN film and an Al film are laminated in order. The gate electrode 303 is not limited to a laminated structure of a TiN film and an Al film, and may be composed of a transition metal nitride or carbide. Specifically, the gate electrode 303 may be composed of TiN, WN, TaN, or HfN. The gate electrode 303 may also be composed of Ti, Ta, W, Al, Pd, Pt, Hf, Ru, and Cu, or may be a compound containing these elements, or may be a multilayer electrode film having a laminated structure of multiple elements. Another insulating layer or a p-type nitride semiconductor layer may be provided between the electron supply layer 104 and the gate electrode 303.

[0046] The electron supply assistance layer 401 is an n-type semiconductor layer made of an n-type semiconductor containing Si. The thickness of the electron supply assistance layer 401 is preferably 2 nm or less, but is not limited to this. In this embodiment, the electron supply assistance layer 401 is an n-AlGaN layer made of n-type AlGaN containing Si and having a thickness of 1 nm.

[0047] The electron supply assistance layer 401 is not in contact with the gate electrode 303, but is in contact with the electron supply layer 104 and the contact layer 212. In a plan view, the electron supply assistance layer 401 is provided between the contact layer 212 and the first insulating layer 201. In a cross-sectional view, the electron supply assistance layer 401 is provided so as to be embedded in the end of the electron supply layer 104 on the contact layer 212 side. Specifically, in a cross-sectional view, the electron supply assistance layer 401 is provided so that its upper surface is flush with the upper surface of the electron supply layer 104 and its lower surface is located between the upper and lower surfaces of the electron supply layer 104.

[0048] In this embodiment, the electron supply assistance layer 401 is in contact with both the source-side contact layer 212A and the drain-side contact layer 212B. Specifically, the electron supply assistance layer 401 is embedded in the end of the electron supply layer 104 on the source-side contact layer 212A side and also embedded in the end of the electron supply layer 104 on the drain-side contact layer 212B side. The electron supply assistance layer 401 may be in contact with only one of the source-side contact layer 212A and the drain-side contact layer 212B. The electron supply assistance layer 401 may also be divided into multiple layers. In this case, the electron supply assistance layer 401 on the source electrode 301 side may be in contact with the source-side contact layer 212A, and the electron supply assistance layer 401 on the drain electrode 302 side may be in contact with the drain-side contact layer 212B.

[0049] The width of the electron supply assistance layer 401 may be smaller than the distance L between the gate electrode 303 and the end of the electron supply assistance layer 401 on the gate electrode 303 side. As an example, the width of the electron supply assistance layer 401 is 1 μm or less in a cross-sectional view. This can efficiently suppress an increase in leakage current between the gate electrode 303 and the drain electrode 302.

[0050] Alternatively, one of the electron supply assist layer 401 on the source electrode 301 side and the electron supply assist layer 401 on the drain electrode 302 side may not be in contact with the gate electrode 303, and the other may be in contact with the gate electrode 303. For example, when the width of the electron supply assist layer 401 on the drain electrode 302 side is within the range of the above-mentioned distance L, the electron supply assist layer 401 on the source electrode 301 side may be in contact with the gate electrode 303. In this way, the access resistance between the source electrode 301 and the gate electrode 303 can be reduced, and therefore the maximum drain current can be increased.

[0051] The alloy layer 402 is provided on the electron supply assistance layer 401, which is an n-type semiconductor layer. Specifically, the alloy layer 402 is provided directly on the electron supply assistance layer 401 and is in contact with the electron supply assistance layer 401.

[0052] The alloy layer 402 is a Si-based alloy layer containing Si. The alloy layer 402 is an alloy layer formed by a reaction between elements constituting the first insulating layer 201 and elements constituting the source electrode 301 and / or drain electrode 302. In this case, the Si constituting the alloy layer 402 is derived from the Si contained in the first insulating layer 201. In this embodiment, the first insulating layer 201 is a SiN layer, and the source electrode 301 and the drain electrode 302 are laminated films of a Ti film and an Al film. Therefore, the alloy layer 402 is an alloy layer composed of Ti, Al, Si, and N. Specifically, the alloy layer 402 is a TiAlSiN alloy layer composed of a TiAlSiN alloy and having a thickness of 1 nm. The thickness of the alloy layer 402 is not limited to 1 nm, but is preferably 2 nm or less. This increases the concentration of Si diffusing into the electron supply layer 104.

[0053] The alloy constituting the alloy layer 402 is not limited to a TiAlSiN alloy, and various combinations of alloys are possible depending on the types of elements constituting the first insulating layer 201 and the types of elements constituting the source electrode 301 and the drain electrode 302. Specifically, the alloy layer 402 may be made of an alloy containing Si and at least one of the elements Ti, Ta, Al, Au, Hf, Ru, and Cu.

[0054] Furthermore, the alloy layer 402 is not in contact with the gate electrode 303 but is in contact with the contact layer 212. In a plan view, the alloy layer 402 is provided between the contact layer 212 and the first insulating layer 201. In this embodiment, the alloy layer 402 is in contact not only with the contact layer 212 but also with the first insulating layer 201.

[0055] In this embodiment, the alloy layer 402 is in contact with both the source-side contact layer 212A and the drain-side contact layer 212B. The alloy layer 402 may be in contact with only one of the source-side contact layer 212A and the drain-side contact layer 212B. The alloy layer 402 may also be divided into a plurality of layers. In this case, the alloy layer 402 on the source electrode 301 side may be in contact with the source-side contact layer 212A, and the alloy layer 402 on the drain electrode 302 side may be in contact with the drain-side contact layer 212B.

[0056] By providing the semiconductor device 1 with such a structure, the electron concentration of the two-dimensional electron gas layer 105 can be made different between a portion where the electron supply assistance layer 401 and the alloy layer 402 are present and a portion where the electron supply assistance layer 401 and the alloy layer 402 are not present. Specifically, the two-dimensional electron gas layer 105 has a first two-dimensional electron gas layer 105A that is not located below the electron supply assistance layer 401 and the alloy layer 402, and a second two-dimensional electron gas layer 105B that is located below the electron supply assistance layer 401 and the alloy layer 402, and the electron concentration of the second two-dimensional electron gas layer 105B is higher than the electron concentration of the first two-dimensional electron gas layer 105A. The contact layer 212 and the second two-dimensional electron gas layer 105B are electrically ohmic-connected.

[0057] Here, the mechanism by which the electron concentration of the second two-dimensional electron gas layer 105B becomes higher than the electron concentration of the first two-dimensional electron gas layer 105A will be described with reference to Fig. 2. Fig. 2 is a schematic diagram showing the conduction band of the energy band of the semiconductor device 1 according to the first embodiment.

[0058] In Fig. 2 , solid line A is a diagram of a portion corresponding to dashed-dotted line A in Fig. 1 , and dashed line B is a diagram of a portion corresponding to dashed-dotted line B in Fig. 1 . That is, solid line A in Fig. 2 is a diagram of a gate-adjacent portion adjacent to the gate electrode 303 (i.e., a portion where the electron supply assistance layer 401 and the alloy layer 402 are not provided), and the names of the corresponding layers are indicated by a row of double-headed arrows (A) on the lower side. Furthermore, dashed line B in Fig. 2 is a diagram of a contact-adjacent portion adjacent to the contact layer 212 (i.e., a portion where the electron supply assistance layer 401 and the alloy layer 402 are provided), and the names of the corresponding layers are indicated by a row of double-headed arrows (B) on the upper side. The dashed line above the electron supply assistance layer 401 (left side in the figure) indicates that the Fermi level of the drain electrode 302, which is a metal, coincides with the conduction band.

[0059] As described above, in the semiconductor device 1 according to the present embodiment, the electron supply assistance layer 401 made of an n-type semiconductor is provided inside the electron supply layer 104. This relatively reduces the potential of the electron supply layer 104 in the portion where the electron supply layer 104 is provided, thereby reducing the potential at the interface between the electron supply layer 104 and the electron transit layer 103. As a result, the electron concentration of the second two-dimensional electron gas layer 105B increases. That is, the electron concentration of the second two-dimensional electron gas layer 105B located below the electron supply assistance layer 401 becomes higher relative to the electron concentration of the first two-dimensional electron gas layer 105A not located below the electron supply assistance layer 401.

[0060] In this manner, the electron concentration of the second two-dimensional electron gas layer 105B is higher than the electron concentration of the first two-dimensional electron gas layer 105A, thereby preventing a decrease in the electron concentration in the portion of the electron supply layer 104 adjacent to the side surface of the through-hole recess 211. As a result, a decrease in the maximum drain current can be suppressed. Moreover, since the electron concentration in the portion adjacent to the gate corresponding to the first two-dimensional electron gas layer 105A is maintained, the leakage current between the gate electrode 303 and the drain electrode 302 can also be reduced. In other words, the configuration of the semiconductor device 1 according to this embodiment can achieve both a reduction in the maximum drain current and a reduction in the leakage current between the gate and the drain. Furthermore, since the current increases not only through the contact layer 212 but also through the electron supply assistance layer 401 and the alloy layer 402, a decrease in the maximum drain current can be further suppressed.

[0061] In the semiconductor device 1 according to the present embodiment, the width of the electron supply assistance layer 401 is preferably 1 μm or less, which can efficiently reduce the leakage current between the gate electrode 303 and the drain electrode 302.

[0062] Furthermore, in the semiconductor device 1 according to the present embodiment, the band gap of the electron supply layer 104 on the electron supply assist layer 401 side below the electron supply assist layer 401 may be smaller than the band gap of the electron supply layer 104 on the electron transit layer 103 side. Specifically, when the electron supply layer 104 is made of AlGaN, the Al composition of the electron supply layer 104 on the electron supply assist layer 401 side may be smaller than the Al composition of the electron supply layer 104 on the electron transit layer 103 side. Since the electron affinity of AlGaN decreases with increasing Al composition, the barrier height decreases when the Si-containing alloy layer 402 is brought into contact with the electron supply assist layer 401. Therefore, by making the band gap of the electron supply layer 104 on the electron supply assist layer 401 side smaller than the band gap of the electron supply layer 104 on the electron transit layer 103 side, the ohmic contact resistance can be reduced. Furthermore, reducing the ohmic contact resistance reduces variations in drain current.

[0063] In the semiconductor device 1 according to the present embodiment, the first insulating layer 201 and the electron supply assistance layer 401 may contain halogen such as fluorine (F) or chlorine (Cl). The halogen concentration in the first insulating layer 201 and the electron supply assistance layer 401 is preferably 1×10 18 atoms / cm 3 This is because halogen contained in the semiconductor layer or insulating layer has high electronegativity and becomes a negative fixed charge. Therefore, the halogen concentration of the first insulating layer 201 is preferably 1×10 or less. 18 atoms / cm 3 or less, it is possible to reduce the negative fixed charges in the first insulating layer 201. This makes it possible to prevent an increase in the potential at the interface between the electron supply layer 104 and the electron transit layer 103, and to prevent a decrease in the electron concentration in the second two-dimensional electron gas layer 105B due to the halogen.

[0064] In the semiconductor device 1 according to the present embodiment, the thickness of the first insulating layer 201 may be greater than the thickness of the alloy layer 402. By doing so, the leakage current between the gate electrode 303 and the drain electrode 302 can be further reduced.

[0065] Next, a manufacturing method of the semiconductor device 1 according to the present embodiment will be described with reference to FIGS. 3A to 3G. FIGS. 3A to 3G are cross-sectional views illustrating respective steps in the manufacturing method of the semiconductor device 1 according to the first embodiment. FIG. 3A illustrates a step of forming the semiconductor stack 100 and the first and second insulating layers 201 and 202. FIG. 3B illustrates a step of forming the thin portion 201b in the first insulating layer 201. FIG. 3C illustrates a step of forming the through-hole recess 211. FIG. 3D illustrates a step of forming the contact layer 212. FIG. 3E illustrates a step of forming the source electrode 301 and the drain electrode 302. FIG. 3F illustrates a heat treatment step. FIG. 3G illustrates a step of forming the gate electrode 303.

[0066] First, as shown in FIG. 3A , a semiconductor stacked structure 100 including a buffer layer 102, an electron transit layer 103, and an electron supply layer 104 is formed on a substrate 101 by metal organic chemical vapor deposition (MOCVD) (semiconductor stacked structure formation step).

[0067] In this embodiment, a semiconductor laminated structure 100 is formed on a substrate 101 made of Si by epitaxially growing, in the +c-plane direction (<0001> direction), a buffer layer 102 having a layer thickness of 2 μm and made of a laminated structure of AlN and AlGaN, an electron transit layer 103 having a layer thickness of 200 nm and made of GaN, and an electron supply layer 104 having a layer thickness of 20 nm and made of AlGaN with an Al composition ratio of 25%.

[0068] Next, a first insulating layer 201 is formed on the semiconductor stack 100 as an insulating layer containing Si (first insulating layer forming step). Specifically, after forming the semiconductor stack 100, the first insulating layer 201 made of SiN and having a thickness of 2 nm is formed in the same semiconductor crystal growth apparatus (MOCVD furnace). That is, the first insulating layer 201 is formed on the electron supply layer 104 without exposure to the atmosphere. In this way, by forming the first insulating layer 201 directly on the electron supply layer 104 without exposure to the atmosphere, oxygen is not unevenly distributed between the electron supply layer 104 and the first insulating layer 201.

[0069] Next, a second insulating layer 202 is formed on the first insulating layer 201 (second insulating layer forming step). Specifically, after the first insulating layer 201 is formed, the semiconductor stack 100 and the substrate 101 on which the first insulating layer 201 is formed are transferred to another device, and a SiO 2 In this structure, a high concentration of two-dimensional electron gas is generated on the electron transit layer 103 side of the heterointerface between the electron supply layer 104 and the electron transit layer 103, forming a two-dimensional electron gas layer 105.

[0070] The film formation conditions for forming the first insulating layer 201 and the second insulating layer 202 are, for example, a growth temperature of 900 to 1150° C. and a source gas of SiH 4 and N.H. 3In addition, in order to prevent halogen from being mixed as an impurity into the first insulating layer 201, it is better not to use halogen when dry cleaning the inside of the MOCVD furnace. Even if halogen is used during dry cleaning, N 2 and NH 3 It is advisable to remove halogens from the MOCVD furnace by using a method such as the above.

[0071] Next, as shown in FIG. 3B, a part of the first insulating layer 201 is thinned to form a thin portion 201b in the first insulating layer 201 (thin portion forming step).

[0072] Specifically, a resist is applied onto the second insulating layer 202, and then the resist is patterned by lithography to form a mask (resist mask) on the second insulating layer 202 in a portion excluding the regions where the contact layer 212, the electron supply assistance layer 401, and the alloy layer 402 are to be formed. That is, openings are formed in the resist in the regions where the contact layer 212, the electron supply assistance layer 401, and the alloy layer 402 are to be formed. Specifically, openings are formed in regions including the regions where the source-side contact layer 212A and the drain-side contact layer 212B are to be formed.

[0073] Next, etching is performed using a resist having openings as a mask to remove a portion of the second insulating layer 202 and thin a portion of the first insulating layer 201. In this case, dry etching and wet etching are performed using the resist having openings as a mask to selectively remove the second insulating layer 202 relative to the first insulating layer 201. That is, by performing dry etching and wet etching, the second insulating layer 202 is removed and the first insulating layer 201 is thinned in the region where the contact layer 212, the electron supply assistance layer 401, and the alloy layer 402 are to be formed. As a result, as shown in FIG. 3B , a portion of the first insulating layer 201 (the region where the contact layer 212, the electron supply assistance layer 401, and the alloy layer 402 are to be formed) is thinned, and a thin portion 201b is formed in the first insulating layer 201 as a remaining film. Then, the mask (resist) and the polymer generated by the dry etching are removed.

[0074] When wet etching is performed on the first insulating layer 201 and the second insulating layer 202, the second insulating layer 202 can be selectively removed with respect to the first insulating layer 201 by using DHF or BHF. 2 When forming the second insulating layer 202 made of the above, the surface of the first insulating layer 201 may be oxidized to selectively remove only a portion of the first insulating layer 201 .

[0075] Furthermore, the thickness of the thin portion 201b (residual film) of the first insulating layer 201 is preferably 2 nm or less. In this case, the thickness of the thin portion 201b (residual film) of the first insulating layer 201 is preferably at least half the thickness of the first insulating layer 201 before thinning (i.e., at least half should be left), but is not limited to this. As an example, if the thickness of the first insulating layer 201 before thinning is 2 nm, the thickness of the thin portion 201b (residual film) of the first insulating layer 201 is 1.5 nm.

[0076] 3C , an end portion of the thin portion 201b of the first insulating layer 201 and a part of the semiconductor stack 100 are removed to form a through-hole recess 211 (through-hole recess forming step). Specifically, the through-hole recess 211 is formed so as to penetrate the thin portion 201b of the first insulating layer 201 and the electron supply layer 104 and reach the electron transit layer 103, while leaving a part of the thin portion 201b of the first insulating layer 201 as the remaining insulating layer 201b1.

[0077] In this case, first, a resist is applied to the second insulating layer 202 and to a part of the thin portion 201b of the first insulating layer 201, and then the resist is patterned by lithography to form a mask (resist mask) in an area other than the area where the through-hole recess 211 is to be formed. That is, the resist has openings in the area where the through-hole recess 211 is to be formed. Specifically, the resist has openings in each of the areas where the source-side contact layer 212A and the drain-side contact layer 212B are to be formed.

[0078] Next, dry etching is performed using the resist with the openings as a mask to form through-hole recesses 211 that penetrate the end of the thin portion 201b of the first insulating layer 201 and the electron supply layer 104 and reach the electron transit layer 103, while leaving a portion of the thin portion 201b of the first insulating layer 201 as the insulating layer remaining portion 201b1. Specifically, as shown in FIG. 3C , two through-hole recesses 211 are formed corresponding to the regions where the source-side contact layer 212A and the drain-side contact layer 212B are to be formed. By forming the through-hole recesses 211, a portion of the electron transit layer 103 is exposed. Then, the mask (resist) and the polymer generated by the dry etching are removed.

[0079] In this embodiment, the through-hole recess 211 is formed by dry etching, but the method is not limited to this. Specifically, the through-hole recess 211 may be formed by wet etching.

[0080] Alternatively, after thinning the first insulating layer 201 and forming the through-hole recess 211 by dry etching, the side surface of the electron supply layer 104 may be selectively wet-etched using SPM, APM, or KOH. This allows the side surface of the through-hole recess 211 to be an inclined surface. Specifically, the side surface of the through-hole recess 211 can be an inclined surface having an elevation angle of 5 degrees or less in the direction from the center of the bottom surface of the through-hole recess 211 to the side.

[0081] Next, as shown in FIG. 3D, a contact layer 212 is formed by filling the through-hole recess portion 211 (contact layer forming step).

[0082] Specifically, the second insulating layer 202 and the remaining insulating layer 201b1 of the first insulating layer 201 are used as a mask to form a n-type insulating film by MOCVD so as to fill the two through-hole recess portions 211. + GaN is grown in each of the two through recesses 211. +The contact layer 212 made of -GaN can be selectively embedded and formed. The contact layer 212 embedded in one of the two through-hole recesses 211 is a source-side contact layer 212A, and the contact layer 212 embedded in the other of the two through-hole recesses 211 is a drain-side contact layer 212B.

[0083] In this embodiment, Si is doped as an n-type impurity, and the n-type + The contact layer 212 was formed by growing GaN. The Si doping concentration of the contact layer 212 was, for example, 2×10 19 / cm 3 The contact layer 212 may be formed by sputtering instead of regrowth, or may be formed by ion implantation and plasma treatment without forming the penetrating recess portion 211.

[0084] Next, as shown in FIG. 3E, a source electrode 301 and a drain electrode 302 are formed across the insulating layer remaining portion 201b1 of the first insulating layer 201 and the contact layer 212 (source electrode / drain electrode forming step).

[0085] Specifically, a 30 nm thick Ti film and a 200 nm thick Al film are sequentially deposited by vapor deposition or sputtering to form a laminated film, and then unnecessary laminated film is removed by lift-off to form source electrode 301 and drain electrode 302 of predetermined shapes made of a laminated film of Ti film and Al film on contact layer 212. In this embodiment, source electrode 301 is formed on source-side contact layer 212A, and drain electrode 302 is formed on drain-side contact layer 212B. Then, the resist mask and polymer are removed.

[0086] In this embodiment, the source electrode 301 and the drain electrode 302 are formed by vapor deposition and lift-off, but the method is not limited to this. For example, a Ti film and an Al film may be deposited in this order by sputtering to form a laminated film, and then the laminated film may be patterned by lithography and dry etching to form the source electrode 301 and the drain electrode 302 in a predetermined shape.

[0087] Next, as shown in FIG. 3F, a heat treatment is performed to form an electron supply auxiliary layer 401 and an alloy layer 402 on the insulating layer remaining portion 201b1 of the first insulating layer 201 and the electron supply layer 104 (heat treatment step).

[0088] The temperature of this heat treatment is, for example, 400 to 600° C., preferably 500 to 550° C. The heat treatment is preferably performed in an atmosphere that does not contain oxygen. 2 The substrate was subjected to a heat treatment at a temperature of 540° C. in an atmosphere.

[0089] By performing heat treatment in this manner, the elements constituting the insulating layer remaining portion 201b1 of the first insulating layer 201 and the electron supply layer 104 and the elements constituting the source electrode 301 and the drain electrode 302 are mutually diffused and alloyed by heat, forming the electron supply auxiliary layer 401 and the alloy layer 402.

[0090] Specifically, in this embodiment, the first insulating layer 201 is an insulating layer containing Si, and the electron supply layer 104 is an AlGaN layer, so that the upper layer portion of the electron supply layer 104 in contact with the insulating layer remaining portion 201b1 of the first insulating layer 201 becomes n-type due to the formation of nitrogen vacancies caused by the diffusion of Si constituting the first insulating layer 201, and an n-type AlGaN layer is formed as the electron supply assistance layer 401. That is, the electron supply assistance layer 401 is formed as an n-type semiconductor layer.

[0091] Moreover, in this embodiment, since the source electrode 301 and the drain electrode 302 contain Ti, the formation of nitrogen vacancies due to the diffusion of this Ti also causes the upper portion of the electron supply layer 104 to become n-type. That is, in this embodiment, the diffusion of Si and Ti due to the heat treatment causes the upper portion of the electron supply layer 104 to become n-type, and the electron supply assistance layer 401, which is an n-type semiconductor layer, is formed.

[0092] In this way, the upper layer portion of the electron supply layer 104 becomes n-type to form the electron supply assistance layer 401, which is an n-type semiconductor layer, thereby generating the second two-dimensional electron gas layer 105B having a higher electron concentration than the first two-dimensional electron gas layer 105A. As a result, the second two-dimensional electron gas layer 105B is electrically connected to the source electrode 301 and the drain electrode 302 in an ohmic contact.

[0093] In order to facilitate diffusion of Si in the first insulating layer 201 to the electron supply layer 104 by heat treatment, it is preferable that the remaining insulating layer portion 201b1, which is a part of the thin portion 201b of the first insulating layer 201, is thin. In this case, as described above, it is preferable that the thickness of the thin portion 201b of the first insulating layer 201 is 2 nm or less. By doing so, it is possible to increase the Si content in the upper layer portion of the electron supply layer 104, and to make the upper layer portion of the electron supply layer 104 more n-type.

[0094] 3G , the first insulating layer 201 is removed from a portion thereof spaced apart from the source electrode 301 and the drain electrode 302 to form the gate electrode 303 (gate electrode formation step). In this embodiment, the second insulating layer 202 is formed on the first insulating layer 201, and therefore the first insulating layer 201 and the second insulating layer 202 are removed from a portion thereof spaced apart from the source electrode 301 and the drain electrode 302 to form the gate electrode 303.

[0095] Specifically, after applying resist to the second insulating layer 202, a mask (resist mask) is formed by lithography in areas other than the area where the gate electrode 303 is to be formed (the area where the gate electrode 303 is to be formed). Next, the second insulating layer 202 and the first insulating layer 201 are selectively removed by dry etching to form an opening 201a in the first insulating layer 201 and an opening 202a in the second insulating layer 202 so that the electron supply layer 104 is exposed. Next, the mask (resist mask) and polymer generated by the dry etching are removed. Thereafter, the gate electrode 303 is formed in the openings 201a and 202a. Specifically, a stacked film is formed by sequentially depositing a 50 nm thick TiN film and a 450 nm thick Al film by sputtering, and then the stacked film is patterned by lithography and dry etching to form the gate electrode 303 having the predetermined shape shown in FIG. 3F. Thereafter, the polymer generated by the mask and dry etching is removed.

[0096] In this way, through the series of steps shown in FIGS. 3A to 3G, the semiconductor device 1 having the structure shown in FIG. 1 is completed.

[0097] Second Embodiment Next, a semiconductor device 2 according to a second embodiment will be described with reference to Fig. 4. Fig. 4 is a cross-sectional view showing the configuration of the semiconductor device 2 according to the second embodiment. Note that the following description will focus on differences from the first embodiment, and description of commonalities will be omitted or simplified.

[0098] The semiconductor device 2 according to the present embodiment differs from the semiconductor device 1 according to the above-described embodiment 1 in the configuration of the source electrode 301A and the drain electrode 302A. Specifically, the source electrode 301A and the drain electrode 302A according to the present embodiment are the same as the source electrode 301 and the drain electrode 302 in the semiconductor device 1 according to the above-described embodiment 1, but are formed of the same material and integrated with the contact layer 212.

[0099] More specifically, the source electrode 301A in this embodiment is the same as the source electrode 301 and the source-side contact layer 212A in the first embodiment, which are made of the same material and integrated together. Also, the drain electrode 302A in this embodiment is the same as the drain electrode 302 and the drain-side contact layer 212B in the first embodiment, which are made of the same material and integrated together. In other words, the semiconductor device 2 according to this embodiment does not have a contact layer made of a semiconductor material.

[0100] In this embodiment, the source electrode 301A and the drain electrode 302A are provided so as to fill the through-hole recess 211. The source electrode 301A and the drain electrode 302A are also provided so as to cover the alloy layer 402 and a portion of the second insulating layer 202. The source electrode 301A and the drain electrode 302A are formed, for example, by a multilayer electrode film having a laminate structure in which a 30 nm-thick Ti film and a 200 nm-thick Al film are laminated in this order, but this is not limited thereto. The source electrode 301A and the drain electrode 302A do not contain Au, but this is not limited thereto. The source electrode 301A and the drain electrode 302A may also be formed from Ti, Ta, Al, Hf, Ru, and Cu.

[0101] The source electrode 301A and the drain electrode 302A configured in this manner are electrically ohmically connected to the second two-dimensional electron gas layer 105B.

[0102] The semiconductor device 2 according to the present embodiment can also achieve the same effects as those of the first embodiment. Specifically, the present embodiment also includes the electron supply assistance layer 401, which is an n-type semiconductor layer, and the alloy layer 402, so that the electron concentration of the second two-dimensional electron gas layer 105B is higher than the electron concentration of the first two-dimensional electron gas layer 105A. This can prevent the electron concentration in the electron supply layer 104 adjacent to the side surface of the through-hole recess 211 from decreasing, thereby suppressing a decrease in the maximum drain current.

[0103] Furthermore, in the semiconductor device 2 according to this embodiment, the source electrode 301A and the drain electrode 302A also function as contact layers, and no contact layer made of a semiconductor material is provided. This eliminates the need for a process for forming the contact layer. Furthermore, in the semiconductor device 2 according to this embodiment, the source electrode 301A and the drain electrode 302A do not contain Au, thereby reducing manufacturing costs.

[0104] Next, a method for manufacturing the semiconductor device 2 according to the present embodiment will be described with reference to FIGS. 5A to 5F. FIGS. 5A to 5F are cross-sectional views illustrating steps in the method for manufacturing the semiconductor device 2 according to the second embodiment. FIG. 5A illustrates a step of forming the semiconductor stack 100, the first insulating layer 201, and the second insulating layer 202. FIG. 5B illustrates a step of forming the thin portion 201b in the first insulating layer 201. FIG. 5C illustrates a step of forming the through-recess portion 211. FIG. 5D illustrates a step of forming the source electrode 301A and the drain electrode 302A. FIG. 5E illustrates a step of performing heat treatment. FIG. 5F illustrates a step of forming the gate electrode 303.

[0105] First, as shown in Fig. 5A, a semiconductor laminated structure 100 including a buffer layer 102, an electron transit layer 103, and an electron supply layer 104 is formed on a substrate 101 by MOCVD (semiconductor laminated structure forming step). This step is the same as the step shown in Fig. 3A in the first embodiment.

[0106] 5B, a portion of the first insulating layer 201 is thinned to form a thin portion 201b in the first insulating layer 201 (thin portion forming step). This step is the same as the step shown in FIG. 3B in the first embodiment.

[0107] 5C , an end portion of the thin portion 201b of the first insulating layer 201 and a portion of the semiconductor stack 100 are removed to form a through-hole recess 211 (through-hole recess forming step). Specifically, the through-hole recess 211 is formed so as to penetrate the thin portion 201b of the first insulating layer 201 and the electron supply layer 104 and reach the electron transit layer 103, while leaving a portion of the thin portion 201b of the first insulating layer 201 as the remaining insulating layer 201b1. This step is the same as the step shown in FIG. 3C in the first embodiment.

[0108] 5D , the source electrode 301A and the drain electrode 302A are embedded in the through-hole recess 211 (source electrode / drain electrode forming step). Specifically, the source electrode 301A and the drain electrode 302A are formed across the remaining insulating layer portion 201b1 of the first insulating layer 201 and the through-hole recess 211.

[0109] In this embodiment, using the second insulating layer 202 and the first insulating layer 201 as masks, a Ti film and an Al film are sequentially deposited by sputtering so as to fill the through-hole recess 211, forming a laminated film, and then a mask is formed by lithography in the region where the source electrode 301A and the drain electrode 302A are to be formed. The region where this mask is formed is a region that straddles the through-hole recess 211, the insulating layer remnant 201b1 of the first insulating layer 201, and the second insulating layer 202 in a plan view. Then, the Al film and the Ti film in the region other than the masked region are removed by dry etching, thereby forming the source electrode 301A and the drain electrode 302A straddling the insulating layer remnant 201b1 of the first insulating layer 201 and the through-hole recess 211. The mask and the polymer are then removed.

[0110] 5E , a heat treatment is performed to form an electron supply auxiliary layer 401 and an alloy layer 402 in the insulating layer remaining portion 201b1 of the first insulating layer 201 and the electron supply layer 104 (heat treatment step). This step is the same as the step shown in FIG. 3F in the first embodiment. That is, by performing the heat treatment, elements constituting the insulating layer remaining portion 201b1 of the first insulating layer 201 and the electron supply layer 104 and elements constituting the source electrode 301A and the drain electrode 302A are mutually diffused and alloyed by heat, thereby forming the electron supply auxiliary layer 401 and the alloy layer 402.

[0111] Next, as shown in Fig. 5F, the first insulating layer 201 is removed from a portion thereof spaced apart from the source electrode 301A and the drain electrode 302A to form the gate electrode 303 (gate electrode formation step). In this embodiment, the second insulating layer 202 is also formed on the first insulating layer 201, so the first insulating layer 201 and the second insulating layer 202 are removed from a portion thereof spaced apart from the source electrode 301A and the drain electrode 302A to form the gate electrode 303. This step is the same as the step shown in Fig. 3G in the first embodiment.

[0112] In this way, through the series of steps shown in FIGS. 5A to 5F, the semiconductor device 2 having the structure shown in FIG. 4 is completed.

[0113] (Modifications) Although the semiconductor device according to the present disclosure has been described above based on the first and second embodiments, the present disclosure is not limited to the first and second embodiments.

[0114] For example, in the first and second embodiments, the electron transit layer 103 and the electron supply layer 104 are made of a group III nitride semiconductor, but this is not limiting. Specifically, the electron transit layer 103 and the electron supply layer 104 may be made of other semiconductor materials, such as a group III arsenide semiconductor.

[0115] In addition, the present disclosure also includes forms obtained by applying various modifications to the above-described embodiments that would occur to those skilled in the art, and forms realized by arbitrarily combining the components and functions of the embodiments within the scope of the present disclosure. Furthermore, the present disclosure also includes any combination of two or more claims from among the multiple claims set forth in the claims at the time of filing, within the scope of technical compatibility. For example, when a dependent claim set forth in the claims at the time of filing is made into a multiple claim or multiple multiple claims that cite all of the superordinate claims within the scope of technical compatibility, the present disclosure also includes all combinations of claims included in that multiple claim or multiple multiple multiple claims.

[0116] The technology disclosed herein can be used in semiconductor devices such as switching transistors used in communication equipment and inverters that require high-speed operation, and power supply circuits, etc. Among these, the technology disclosed herein is particularly useful for high-frequency power devices that have a significant impact on heat generation due to ohmic contact resistance.

[0117] 1, 2 Semiconductor device 100 Semiconductor laminated structure 101 Substrate 102 Buffer layer 103 Electron transit layer 104 Electron supply layer 105 Two-dimensional electron gas layer 105A First two-dimensional electron gas layer 105B Second two-dimensional electron gas layer 201 First insulating layer 201a Opening 201b Thin portion 201b1 Remaining portion of insulating layer 202 Second insulating layer 202a Opening 211 Penetrating recess portion 212 Contact layer 212A Source-side contact layer 212B Drain-side contact layer 301, 301A Source electrode 302, 302A Drain electrode 303 Gate electrode 401 Electron supply assistance layer 402 Alloy layer

Claims

a gate electrode provided on the electron supply layer; a source side contact layer and a drain side contact layer embedded in recesses penetrating the electron supply layer at positions on either side of the gate electrode; an n-type semiconductor layer made of an n-type semiconductor containing Si, in contact with the electron supply layer, in contact with the source side contact layer and / or the drain side contact layer but not in contact with the gate electrode; an alloy layer containing Si and having a thickness of 2 nm or less provided on the n-type semiconductor layer; an insulating layer provided on a portion of the electron supply layer where the gate electrode is not provided, in contact with the gate electrode but not in contact with the source side contact layer and / or the drain side contact layer; and a source electrode and / or a drain electrode provided on the source side contact layer and / or the drain side contact layer and on the alloy layer.

2. The semiconductor device according to claim 1, wherein the thickness of the n-type semiconductor layer is 2 nm or less.

3. The semiconductor device according to claim 1 or 2, wherein the width of the n-type semiconductor layer in a cross-sectional view is 1 μm or less.

4. The semiconductor device according to claim 1 or 2, wherein, beneath the n-type semiconductor layer, a band gap of a portion of the electron supply layer on the n-type semiconductor layer side is smaller than a band gap of a portion of the electron supply layer on the electron transit layer side.

5. The semiconductor device according to claim 1 or 2, wherein the source electrode and the source side contact layer are made of the same material and do not contain Au, and the drain electrode and the drain side contact layer are made of the same material and do not contain Au.

6. The insulating layer has a halogen concentration of 1×10 18 atoms / cm 3 The semiconductor device according to claim 1 , wherein:

7. The semiconductor device according to claim 1 or 2, wherein the thickness of said insulating layer is greater than the thickness of said alloy layer.

8. The semiconductor device according to claim 7, wherein the insulating layer has a thickness of 2 nm or more and 30 nm or less.

9. The semiconductor device according to claim 1, wherein there is no uneven distribution of oxygen between said insulating layer and said electron supply layer.

10. The semiconductor device according to claim 1 or 2, wherein the electron transit layer and the electron supply layer are made of a Group III nitride semiconductor.

11. A method for manufacturing a semiconductor device, comprising the steps of: forming an electron supply layer on an electron transit layer, the electron supply layer having a band gap larger than that of the electron transit layer; forming an insulating layer containing Si on the electron supply layer without exposing the insulating layer to the atmosphere; thinning a portion of the insulating layer to form a thin portion in the insulating layer; forming a through recess that penetrates the thin portion of the insulating layer and the electron supply layer to reach the electron transit layer while leaving a portion of the thin portion as a remaining insulating layer; embedding a contact layer in the through recess; forming a source electrode and / or a drain electrode across the remaining insulating layer and the contact layer; 12. A method for manufacturing a semiconductor device, comprising the steps of: forming an electron supply layer on an electron transit layer, the electron supply layer having a band gap larger than that of the electron transit layer; forming an insulating layer containing Si on the electron supply layer without exposing the insulating layer to the atmosphere; thinning a portion of the insulating layer to form a thin portion in the insulating layer; forming a through recess that penetrates the thin portion of the insulating layer and the electron supply layer to reach the electron transit layer while leaving a portion of the thin portion as an insulating layer remnant; forming a source electrode and / or a drain electrode across the insulating layer remnant and the through recess; performing a heat treatment to form an alloy layer and an electron supply auxiliary layer in the insulating layer remnant and the electron supply layer; and removing the insulating layer from a portion of the insulating layer spaced apart from the source electrode and / or the drain electrode to form a gate electrode.

13. The method for manufacturing a semiconductor device according to claim 11 or 12, wherein the insulating layer is made of SiN.

14. The method for manufacturing a semiconductor device according to claim 13, wherein there is no uneven distribution of oxygen between the insulating layer and the electron supply layer.

15. The method for manufacturing a semiconductor device according to claim 11 or 12, wherein in the step of forming a thin portion in the insulating layer, the thickness of the thin portion is 2 nm or less.

16. The method for manufacturing a semiconductor device according to claim 11 or 12, wherein the electron transit layer and the electron supply layer are made of a Group III nitride semiconductor.

Citation Information

Patent Citations

  • Compound semiconductor device and manufacturing method of the same

    JP2015090927A

  • Compound semiconductor device and manufacturing method of the same

    JP2017022214A

  • Compound semiconductor device and manufacturing method thereof

    JP2019012783A

  • Manufacturing method of nitride semiconductor device

    JP2019096774A

  • Method for manufacturing semiconductor device

    JP2020013964A