Electrophotographic photoreceptor, electrophotographic photoreceptor cartridge, and imaging device
The introduction of a polymer with specific structural features in the protective layer of an electrophotographic photoreceptor addresses image blurring and mechanical strength issues, enhancing Martens hardness and preventing particle aggregation for improved performance.
Patent Information
- Application Number
- PCT/JP2024/012661
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional electrophotographic photoreceptors experience image blurring due to the use of initiators with an oxime ester structure, which affects the mechanical strength and abrasion resistance of the photoreceptor surface.
An electrophotographic photoreceptor with a photosensitive layer and a protective layer sequentially on a conductive support, where the protective layer contains a polymer with specific structural formulas, including a compound with a carbazole skeleton, to enhance Martens hardness and elastic deformation rate, and prevent image blurring.
The solution provides a photoreceptor with improved Martens hardness and elastic deformation rate, reducing image blurring and maintaining mechanical strength, while suppressing the aggregation of metal oxide particles.
Smart Images

Figure JP2024012661_03102024_PF_FP_ABST
Abstract
Description
Electrophotographic photoreceptor, electrophotographic photoreceptor cartridge and image forming apparatus
[0001] The present invention relates to an electrophotographic photoreceptor used in a copying machine, a printer, etc., and an electrophotographic photoreceptor cartridge and an image forming apparatus using the same.
[0002] In printers, copiers, and the like, when a charged organic photoconductor (OPC) drum is irradiated with light, the part is discharged, an electrostatic latent image is formed, and an image is obtained by attaching toner to the electrostatic latent image. In such devices that use electrophotography, the photoconductor is a key component.
[0003] Because this type of organic photoreceptor offers a wide range of material options and allows for easy control of photoreceptor properties, "function-separated photoreceptors," in which the functions of charge generation and transport are shared by separate compounds, have become mainstream. For example, known electrophotographic photoreceptors include a single-layer electrophotographic photoreceptor (hereinafter referred to as a single-layer photoreceptor) that contains a charge generation material (CGM) and a charge transport material (CTM) in the same layer, and a multi-layer electrophotographic photoreceptor (hereinafter referred to as a multi-layer photoreceptor) that comprises a charge generation layer containing a charge generation material (CGM) and a charge transport layer containing a charge transport material (CTM). Furthermore, photoreceptor charging methods include a negative charging method, in which the photoreceptor surface is negatively charged, and a positive charging method, in which the photoreceptor surface is positively charged. Currently available photoreceptor layer configuration and charging method combinations include a "negatively charged multi-layer photoreceptor" and a "positively charged single-layer photoreceptor."
[0004] A "negatively charged laminated photoreceptor" generally has a structure in which an undercoat layer (UCL) made of a resin or the like is provided on a conductive substrate such as an aluminum tube, on which a charge generation layer (CGL) made of a charge generation material (CGM) and a resin or the like is provided, and on which a charge transport layer (CTL) made of a hole transport material (HTM) and a resin or the like is provided.
[0005] On the other hand, a "positively charged single-layer photoreceptor" generally has a configuration in which an undercoat layer (UCL) made of a resin or the like is provided on a conductive substrate such as an aluminum tube, and a single-layer photosensitive layer made of a charge generating material (CGM), a hole transporting material (HTM), an electron transporting material (ETM), and a resin or the like is provided thereon (see, for example, Patent Document 1).
[0006] In either case, the surface of the photoreceptor is charged using corona discharge or contact, and then exposed to light to neutralize the surface charge, forming an electrostatic latent image due to the potential difference with the surrounding surface. Toner is then brought into contact with the photoreceptor surface to form a toner image corresponding to the electrostatic latent image, which is then transferred to paper or other media and heated to fuse and fix it to create a print.
[0007] As described above, the basic structure of an electrophotographic photoreceptor is a photosensitive layer formed on a conductive support, but a protective layer may also be provided on the photosensitive layer for the purpose of improving abrasion resistance, etc.
[0008] As a technique for improving the mechanical strength or abrasion resistance of a photoreceptor surface, a photoreceptor has been disclosed in which a protective layer containing a compound having a chain-polymerizable functional group is formed as the outermost layer of the photoreceptor, and this is polymerized by applying energy such as heat, light, or radiation to form a cured resin layer (see, for example, Patent Documents 1 and 2). Compounds having an oxime ester structure are known as highly sensitive photoinitiators used in such protective layers, particularly photocurable protective layers (see, for example, Patent Documents 3, 4, and 5). Among initiators having an oxime ester structure, compounds having a carbazole skeleton also exhibit high sensitivity.
[0009] US Patent No. 9417538 International Publication No. 2010 / 035683 (Patent No. 5263296) JP 2008-216297 A JP 2018-13676 A JP 2020-99008 A
[0010] However, as mentioned above, it has become clear that the use of conventional initiators having an oxime ester structure tends to worsen image flow (image blur).
[0011] An object of the present invention is to provide a new electrophotographic photoreceptor having a photosensitive layer and a protective layer successively formed on a conductive support, which has a high Martens hardness and elastic deformation rate on the surface of the photoreceptor and can reduce image deletion, as well as an electrophotographic photoreceptor cartridge and an image forming apparatus using the electrophotographic photoreceptor.
[0012] In order to solve the above problems, the gist of the present invention resides in the following [1] to
[18] .
[0013] [1] An electrophotographic photoreceptor having a photosensitive layer and a protective layer sequentially formed on a conductive support, wherein the protective layer contains a polymer having a structure represented by the following formula (1):
[0014] [Formula (1)]
[0015] In formula (1), R represents an organic group having two or more carbon atoms. R represents a single bond or a carbonyl group. X, Y, and R 3 each independently represents an arbitrary substituent, and T represents a bond to an arbitrary atom.
[0016] [2] The electrophotographic photoreceptor according to [1], wherein the protective layer contains a polymer having a structure represented by the following formula (2):
[0017] [Formula (2)]
[0018] In formula (2), R1 represents an organic group having two or more carbon atoms. R2 represents a single bond or a carbonyl group. R3, R4, R5, R6, and R7 each independently represent a hydrogen atom, a halogen atom, a nitro group, an acyl group which may have a substituent, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group which may have a substituent, and may be bonded to each other to form a cyclic structure. Y each independently represent a hydrogen atom, a halogen atom, a nitro group, an acyl group which may have a substituent, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group which may have a substituent. T represents a bond to any atom.
[0019] [3] An electrophotographic photoreceptor having a photosensitive layer and a protective layer sequentially provided on a conductive support, wherein the protective layer contains a polymer of a compound represented by the following formula (3):
[0020] [Formula (3)]
[0021] In formula (3), R represents an organic group having two or more carbon atoms. R represents a single bond or a carbonyl group. X, Y, and R 3 each independently represents an arbitrary substituent.
[0022] [4] The electrophotographic photoreceptor according to [3], wherein the protective layer contains a polymer of a compound represented by the following formula (4):
[0023] [Formula (4)]
[0024] In formula (4), R1 represents an organic group having two or more carbon atoms. R2 represents a single bond or a carbonyl group. R3, R4, R5, R6, and R7 each independently represent a hydrogen atom, a halogen atom, a nitro group, an acyl group which may have a substituent, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group which may have a substituent, and may be bonded to each other to form a cyclic structure. Y each independently represent a hydrogen atom, a halogen atom, a nitro group, an acyl group which may have a substituent, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group which may have a substituent. R8 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group which may have a substituent.
[0025] [5] The electrophotographic photoreceptor according to [2] or [4], wherein at least one of R3, R4, R5, R6 and R7 is an acyl group which may have a substituent.
[0026] [6] The electrophotographic photoreceptor according to [5], wherein the acyl group which may have a substituent has a structure represented by formula (5):
[0027] [Formula (5)]
[0028] In formula (5), R9 represents a hydrogen atom, a halogen atom, a nitro group, an acyl group which may have a substituent, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group which may have a substituent. When there are two or more R9s, they may be bonded to each other to form a cyclic structure. U represents a nitrogen atom to which R3 is bonded, or a bond to a carbon atom to which any of R4, R5, R6, and R7 is bonded.
[0029] [7] The electrophotographic photoreceptor according to any one of [1] to [6], wherein the protective layer has a chain-polymerizable functional group. [8] The electrophotographic photoreceptor according to [7], wherein the chain-polymerizable functional group is an acryloyloxy group or a methacryloyloxy group.
[0030] [9] The electrophotographic photoreceptor according to [2], [4], [5] or [6], wherein R6 is a structure represented by formula (5).
[0031]
[10] The R 1 The electrophotographic photoreceptor according to any one of [1] to [9], wherein the organic group is an acyl group which may have a substituent, an alkyl group which may have a substituent, or an aryl group which may have a substituent.
[0032]
[11] The electrophotographic photoreceptor according to any one of [1] to [9], wherein R1 is one structure selected from the group consisting of the following formulas (6) to (8):
[0033] [Formula (6)]
[0034] [Formula (7)]
[0035] [Formula (8)]
[0036] In formulas (6), (7) and (8), W represents a bond to the carbon atom to which R1 is bonded.
[0037]
[12] The R 3
[12] The electrophotographic photoreceptor according to any one of [1] to
[11] , wherein is an alkyl group having 1 to 20 carbon atoms which may have a substituent.
[0038]
[13] The electrophotographic photoreceptor according to any one of [1] to
[11] , wherein the protective layer contains metal oxide particles.
[14] The electrophotographic photoreceptor according to
[13] , wherein the metal oxide particles are titanium oxide.
[15] The electrophotographic photoreceptor according to
[13] , wherein the protective layer contains the structure represented by formula (1) in a proportion of 0.03 mol % to 2 mol % relative to 100 mol % of the metal oxide particles in the protective layer.
[0039]
[16] The electrophotographic photoreceptor according to any one of [1] to
[15] , wherein the photosensitive layer is a single-layer type photosensitive layer.
[0040]
[17] An electrophotographic photosensitive member cartridge having the electrophotographic photosensitive member according to any one of [1] to
[16] .
[18] An image forming apparatus having the electrophotographic photosensitive member according to any one of [1] to
[16] .
[0041] The electrophotographic photoreceptor of the present invention has a high Martens hardness and elastic deformation rate on the surface of the photoreceptor, and can also suppress image deletion.
[0042] 1 is a diagram illustrating an example of the configuration of an image forming apparatus that can be configured using an electrophotographic photosensitive member according to an embodiment of the present invention, and FIG. 2 is a graph illustrating a general relationship between the indentation depth of an indenter and a load curve when measuring the Martens hardness and elastic deformation rate of a photosensitive member.
[0043] The following describes in detail the mode for carrying out the present invention (hereinafter referred to as "embodiments of the invention"). Note that the present invention is not limited to the following embodiments, and various modifications can be made within the scope of the invention.
[0044] <<Present Electrophotographic Photoreceptor>> An electrophotographic photoreceptor according to one example of an embodiment of the present invention (also referred to as “present electrophotographic photoreceptor”) is an electrophotographic photoreceptor including a photosensitive layer and a protective layer sequentially provided on a conductive support, and the protective layer preferably contains a cured product obtained by curing a curable compound.
[0045] The electrophotographic photoreceptor may optionally have layers other than the photosensitive layer and the protective layer. The charging method of the electrophotographic photoreceptor may be either a negative charging method in which the photoreceptor surface is negatively charged or a positive charging method in which the photoreceptor surface is positively charged.
[0046] In the present electrophotographic photoreceptor, the side opposite to the conductive support is the upper side or front side, and the conductive support side is the lower side or back side. From the viewpoint of obtaining the effects of the present invention more effectively, it is preferable that the protective layer is the outermost layer.
[0047] <Protective Layer> The protective layer of the electrophotographic photoreceptor (also referred to as "protective layer") preferably contains a polymer having a structure represented by the following formula (1), and more preferably has a structure represented by the following formula (2).
[0048] [Formula (1)]
[0049] [Formula (2)]
[0050] An example of a case in which the protective layer has a structure represented by formula (1) or (2) above is one in which the protective layer contains a polymer of a compound represented by formula (3) or (4) below. That is, the compound represented by formula (3) or (4) below functions as a polymerization initiator, and therefore, for example, when a curable compound described below is cured, in other words, when crosslinked, a polymer is formed in which the compound represented by formula (3) or (4) below is incorporated into a part of the crosslinked structure, resulting in a structure represented by formula (1) or (2). It is believed that the use of the compound represented by formula (3) or (4) below as a polymerization initiator increases the radical generation efficiency and sufficiently progresses the polymerization reaction, thereby increasing the Martens hardness and elastic deformation rate of the photoreceptor surface.
[0051] [Formula (3)]
[0052] [Formula (4)]
[0053] In formulas (1) to (4), R1 represents an organic group having two or more carbon atoms. Among these, from the viewpoint of acting as a steric hindrance and suppressing image deletion, an organic group having three or more carbon atoms is preferred, an organic group having four or more carbon atoms is more preferred, an organic group having seven or more carbon atoms is more preferred, and an organic group having nine or more carbon atoms is even more preferred. Examples of the organic group include an acyl group which may have a substituent, an alkyl group which may have a substituent, and an aryl group which may have a substituent. Among these, an aryl group which may have a substituent is preferred from the viewpoint of being effective as a steric hindrance.
[0054] An example of the structure of R1 is one selected from the group consisting of the following formulas (6) to (8). Among them, from the viewpoint of steric hindrance, formula (7) or formula (8) is preferred, and formula (8) is more preferred.
[0055] [Formula (6)]
[0056] [Formula (7)]
[0057] [Formula (8)]
[0058] In formulas (6), (7) and (8), W represents a bond to the carbon atom to which R1 is bonded.
[0059] In formulas (1) to (4), R2 represents a single bond or a carbonyl group. Among these, a single bond is preferred from the viewpoint of the stability of the compound.
[0060] In formula (1) and formula (3), X, Y and R 3 Since the substituents X, Y and R do not affect the steric hindrance around the oxime ester moiety, any substituent can be used. 3 is preferably a non-polar substituent. The non-polar substituents are preferably each independently a hydrogen atom, a halogen atom, a nitro group, an acyl group which may have a substituent, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group which may have a substituent. In addition, the optional substituents may be bonded to each other to form a cyclic structure.
[0061] In formula (2) and formula (4), R3, R4, R5, R6, and R7 each independently represent a hydrogen atom, a halogen atom, a nitro group, an acyl group which may have a substituent, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group which may have a substituent, and may be bonded to each other to form a cyclic structure. Among these, from the viewpoint of reactivity, it is preferable that at least one of R3, R4, R5, R6, and R7 is an acyl group which may have a substituent. Among these, R 6 is more preferably an acyl group which may have a substituent.
[0062] From the viewpoint of reactivity, the acyl group which may have a substituent preferably has a structure represented by formula (5). In particular, from the viewpoint of reactivity, it is more preferable that R6 has a structure represented by formula (5).
[0063] [Formula (5)]
[0064] In formula (5), R 9 represents a hydrogen atom, a halogen atom, a nitro group, an acyl group which may have a substituent, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group which may have a substituent. 9 When two or more of these are present, they may be bonded to each other to form a cyclic structure. U represents a bond to the nitrogen atom to which R3 is bonded, or to the carbon atom to which any of R4, R5, R6, and R7 is bonded.
[0065] In the present invention, the phrase "may have a substituent" means that the compound can have a substituent, and includes both cases where the compound has a substituent and cases where the compound does not have a substituent. Furthermore, the "substituent" used here means any atom or atomic group that can replace a hydrogen atom in the structure. Examples of the substituent include a halogen atom, a hydroxy group, an alkyl group, an alkoxy group, an acyl group, a carboxy group, an aryl group, a phenyl group, an amino group, an amide group, a nitro group, a cyano group, and a thiol group. When the compound has a substituent, the substituent is preferably an alkyl group.
[0066] In formula (2) and formula (4), each Y independently represents a hydrogen atom, a halogen atom, a nitro group, an acyl group which may have a substituent, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group which may have a substituent.
[0067] In formula (1) and formula (2), T represents a bond to any atom. T represents a bond to a counterpart structure with which the compound represented by formula (2) is polymerized.
[0068] In formula (3), R8 represents an arbitrary substituent. In formula (4), R8 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group which may have a substituent. Of these, from the viewpoint of reactivity, R8 is preferably an alkyl group having 1 to 20 carbon atoms which may have a substituent. Of these, an alkyl group having 1 to 6 carbon atoms is preferred, an alkyl group having 1 to 3 carbon atoms is more preferred, and an alkyl group having 1 carbon atom, i.e., a methyl group, is even more preferred.
[0069] (Metal Oxide Particles) The protective layer preferably contains metal oxide particles from the viewpoint of imparting charge transport ability and improving mechanical strength.
[0070]
[0013] Note that when a protective layer contains metal oxide particles together with a conventional polymerization initiator having an oxime ester structure, the metal oxide particles tend to aggregate, resulting in image deletion. This is presumably because the oxime ester moiety of the polymerization initiator adsorbs to the surface of the metal oxide particles, suppressing the electrostatic repulsion between the metal oxide particles and causing aggregation, resulting in image deletion. In contrast, when a compound having an oxime ester structure with the above-described substituent R1 is used as a polymerization initiator as in the present invention, the substituent R1 acts as a steric hindrance, inhibiting adsorption of the oxime ester moiety to the surface of the metal oxide particles, thereby suppressing aggregation of the metal oxide particles and preventing image deletion.
[0071] The metal oxide particles can be metal oxide particles that can be used in electrophotographic photoreceptors. Examples of metal oxide particles include metal oxide particles containing one metal element such as titanium oxide, tin oxide, aluminum oxide, silicon oxide, zirconium oxide, indium oxide, zinc oxide, and iron oxide, and metal oxide particles containing multiple metal elements such as indium tin oxide, calcium titanate, strontium titanate, and barium titanate. Only one type of metal oxide particle may be used, or multiple types of particles may be mixed and used. Among these metal oxide particles, metal oxide particles having a band gap of 2 to 4 eV are preferred from the viewpoint of preventing image deletion. Examples of metal oxide particles having a band gap of 2 to 4 eV include metal oxide particles containing one metal element such as titanium oxide, tin oxide, indium oxide, zinc oxide, and iron oxide, and metal oxide particles such as indium tin oxide, calcium titanate, strontium titanate, and barium titanate. Among these metal oxide particles, titanium oxide, tin oxide, indium tin oxide, and zinc oxide are preferred, and titanium oxide or tin oxide is more preferred from the viewpoint of electron transport properties. Among these, titanium oxide is particularly preferred from the viewpoint of easily achieving a balance between image deletion suppression and electrical properties.
[0072] The crystalline form of the titanium oxide particles may be any of rutile, anatase, brookite, and amorphous. Also, the titanium oxide particles may have different crystalline forms, and may contain a plurality of crystalline forms.
[0073] The surfaces of the metal oxide particles may be subjected to various surface treatments. For example, they may be treated with inorganic substances such as tin oxide, aluminum oxide, antimony oxide, zirconium oxide, and silicon oxide, or organic substances such as stearic acid, polyols, and organosilicon compounds. In particular, when titanium oxide particles are used, it is preferable that the particles be surface-treated with an organosilicon compound. Examples of the organosilicon compound include silicone oils such as dimethylpolysiloxane and methylhydrogenpolysiloxane, organosilanes such as methyldimethoxysilane and diphenyldidimethoxysilane, silazanes such as hexamethyldisilazane, and silane coupling agents such as 3-methacryloyloxypropyltrimethoxysilane, 3-acryloyloxypropyltrimethoxysilane, vinyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, and γ-aminopropyltriethoxysilane. In particular, from the viewpoint of improving the mechanical strength of the protective layer, 3-methacryloyloxypropyltrimethoxysilane, 3-acryloyloxypropyltrimethoxysilane, and vinyltrimethoxysilane, which have a chain-polymerizable functional group, are preferred. Note that the outermost surfaces of these surface-treated particles may be treated with a treating agent such as aluminum oxide, silicon oxide, or zirconium oxide before being treated with such a treating agent.
[0074] The particle size of the metal oxide particles is preferably an average primary particle size of 500 nm or less, more preferably 100 nm or less, and even more preferably 50 nm or less. It is also more preferably 1 nm or more, and even more preferably 5 nm or more. This average primary particle size can be determined by the arithmetic mean value of particle diameters directly observed with a transmission electron microscope (hereinafter also referred to as TEM).
[0075] From the viewpoint of electrical properties, the content of the metal oxide particles in the protective layer is preferably 20 parts by mass or more, more preferably 60 parts by mass or more, and even more preferably 80 parts by mass or more, relative to 100 parts by mass of the polymer contained in the protective layer, while from the viewpoint of maintaining the surface charge, the content is preferably 200 parts by mass or less, more preferably 160 parts by mass or less, and even more preferably 120 parts by mass or less.
[0076] When the protective layer contains metal oxide particles, the content of the structure represented by formula (1) in the protective layer is preferably 0.03 mol% or more and 2 mol% or less relative to 100 mol% of the metal oxide particles. If the content of the structure represented by formula (1) is 0.03 mol% or more relative to 100 mol% of the metal oxide particles, this is preferred from the viewpoint of forming a highly hardened film. From this viewpoint, the content of the structure represented by formula (1) is more preferably 0.1 mol% or more, more preferably 0.3 mol% or more, and even more preferably 0.6 mol% or more. On the other hand, if the content of the structure represented by formula (1) is 2 mol% or less relative to 100 mol% of the metal oxide particles, this is preferred because the electrical properties are good. From this viewpoint, the content of the structure represented by formula (1) is more preferably 1.5 mol% or less, more preferably 1.2 mol% or less, and even more preferably 1 mol% or less.
[0077] (Other Materials) In addition to the above materials, the protective layer may contain other materials as needed. For example, the other materials may include a "charge transport material" from the viewpoint of enhancing charge transportability, and may also include, as needed, "another polymerization initiator" different from the compound represented by formula (3) or (4). Furthermore, as needed, the protective layer may include, for example, a stabilizer (heat stabilizer, ultraviolet absorber, light stabilizer, antioxidant, etc.), a dispersant, an antistatic agent, a colorant, a lubricant, etc. These may be used alone or in any combination and ratio.
[0078] [Charge Transport Material] The charge transport material, that is, the charge transport material contained in the protective layer, may be the same as the charge transport material used in the photosensitive layer, which will be described later.
[0079] Furthermore, from the viewpoint of improving the Martens hardness of the photoreceptor surface, it is preferable that the protective layer contains a structure formed by polymerizing a charge transport material having a chain-polymerizable functional group, so that the protective layer has the chain-polymerizable functional group. Examples of the chain-polymerizable functional group of the charge transport material having the chain-polymerizable functional group include an acryloyl group, an acryloyloxy group, a methacryloyl group, a methacryloyloxy group, a vinyl group, and an epoxy group. Among these, from the viewpoint of curability, an acryloyl group, an acryloyloxy group, a methacryloyl group, or a methacryloyloxy group is preferred. The structure of the charge transport material portion of the charge transport material having the chain-polymerizable functional group is preferably a carbazole derivative, an arylamine derivative, a stilbene derivative, a butadiene derivative, or an enamine derivative, or a combination of two or more of these compounds.
[0080] The content of the charge transport material in the protective layer of the electrophotographic photoreceptor is not particularly limited. From the viewpoint of electrical properties, it is preferably 100 parts by mass or more, more preferably 300 parts by mass or more, and even more preferably 500 parts by mass or more, relative to 100 parts by mass of the compound represented by formula (3) or formula (4). Furthermore, from the viewpoint of maintaining good surface resistance, it is more preferably 5000 parts by mass or less, more preferably 3000 parts by mass or less, and even more preferably 2000 parts by mass or less.
[0081] [Polymerization initiator] The compound represented by formula (3) or (4) functions as a polymerization initiator, particularly a photopolymerization initiator that generates radicals upon irradiation with light. Therefore, it is not necessary to contain a polymerization initiator other than the compound represented by formula (3) or (4) (referred to as "other polymerization initiators"). However, if necessary, the compound may contain "other polymerization initiators." In this case, "other polymerization initiators" include thermal polymerization initiators, photopolymerization initiators, etc.
[0082] Examples of the thermal polymerization initiator include peroxide compounds such as 2,5-dimethylhexane-2,5-dihydroperoxide, and azo compounds such as 2,2'-azobis(isobutyronitrile).
[0083] Photopolymerization initiators can be classified into direct cleavage type and hydrogen abstraction type depending on the radical generation mechanism.
[0084] Examples of the direct cleavage type photopolymerization initiator include acetophenone or ketal compounds such as acetophenone, 2-benzoyl-2-propanol, 1-benzoylcyclohexanol, 2,2-diethoxyacetophenone, benzyl dimethyl ketal, and 2-methyl-4'-(methylthio)-2-morpholinopropiophenone; benzoin ether compounds such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isobutyl ether, benzoin isopropyl ether, and O-tosylbenzoin; and acylphosphine oxide compounds such as diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, and lithium phenyl(2,4,6-trimethylbenzoyl)phosphonate.
[0085] Examples of hydrogen abstraction photopolymerization initiators include benzophenone compounds such as benzophenone, 4-benzoylbenzoic acid, 2-benzoylbenzoic acid, methyl 2-benzoylbenzoate, methyl benzoylformate, benzyl, p-anisil, 2-benzoylnaphthalene, 4,4'-bis(dimethylamino)benzophenone, 4,4'-dichlorobenzophenone, and 1,4-dibenzoylbenzene, and anthraquinone or thioxanthone compounds such as 2-ethylanthraquinone, 2-isopropylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, and 2,4-dichlorothioxanthone. Other examples of photopolymerization initiators include camphorquinone, 1-phenyl-1,2-propanedione-2-(o-ethoxycarbonyl)oxime, acridine compounds, triazine compounds, and imidazole compounds.
[0086] In order to efficiently absorb light energy and generate radicals, the photopolymerization initiator preferably has an absorption wavelength in the wavelength region of the light source used for light irradiation. From the viewpoint of preventing a decrease in radical generation efficiency, it is preferable to contain an acylphosphine oxide-based compound, which has an absorption wavelength on the relatively long wavelength side among photopolymerization initiators. In this case, from the viewpoint of enhancing the curability of the surface of the protective layer, it is more preferable to use an acylphosphine oxide-based compound in combination with a hydrogen abstraction initiator. The content ratio of the hydrogen abstraction initiator relative to the acylphosphine oxide-based compound is not particularly limited. For example, from the viewpoint of enhancing surface curability, it is preferable to contain 0.1 parts by mass or more of the hydrogen abstraction initiator per 1 part by mass of the acylphosphine oxide-based compound, and from the viewpoint of maintaining internal curability, it is preferable to contain 5 parts by mass or less of the hydrogen abstraction initiator.
[0087] Furthermore, a compound having a photopolymerization promoting effect can be used alone or in combination with the above photopolymerization initiator. Examples of compounds having a photopolymerization promoting effect include triethanolamine, methyldiethanolamine, ethyl 4-dimethylaminobenzoate, isoamyl 4-dimethylaminobenzoate, (2-dimethylamino)ethyl benzoate, and 4,4'-dimethylaminobenzophenone.
[0088] The polymerization initiator may be used alone or in combination of two or more. The content of the polymerization initiator is preferably 0.5 to 40 parts by mass, more preferably 1 part by mass or more or 20 parts by mass or less, per 100 parts by mass of the total content of radically polymerizable compounds.
[0089] Whether the protective layer has a structure represented by formula (1) or (2) and whether the protective layer contains a polymer of a compound represented by formula (3) or (4) can be determined, for example, by pyrolyzing the protective layer and then using GC-MS or the like. The content ratios of each component contained in the protective layer can also be measured, for example, by pyrolyzing the protective layer and then using GC-MS or the like. Specifically, when signals derived from the structures of formulas (9) to (18) below are detected by pyrolysis GC-MS analysis, it can be determined that the protective layer has a structure represented by formula (1) or (2) or contains a polymer of a compound represented by formula (3) or (4).
[0090]
[0091] (Method for forming the protective layer) Next, a method for forming the protective layer will be described. The method for forming the protective layer is not particularly limited. For example, the protective layer can be formed by applying a coating liquid (referred to as the "coating liquid for forming the protective layer") prepared by dissolving the compound having the structure represented by formula (3) or (4) together with the curable compound described below, and optionally further including the metal oxide particles, and optionally further including the other polymerization initiator, the charge transport material, and optionally further including other substances in a solvent or a dispersion medium, onto the photosensitive layer and curing the coating liquid.
[0092] [Curable Compound] Examples of the curable compound include a monomer, oligomer, or polymer having a chain-polymerizable functional group. Among these, a crosslinkable curable compound, particularly a photocurable compound, is preferred. For example, a curable compound having two or more chain-polymerizable functional groups can be used. A compound having one chain-polymerizable functional group can also be used in combination. In this way, by using a curable compound having a chain-polymerizable functional group, the protective layer can also have a chain-polymerizable functional group. Examples of the chain-polymerizable functional group include an acryloyl group, an acryloyloxy group, a methacryloyl group, a methacryloyloxy group, a vinyl group, and an epoxy group. Among these, an acryloyl group, an acryloyloxy group, a methacryloyl group, or a methacryloyloxy group is preferred, and an acryloyloxy group or a methacryloyloxy group is more preferred.
[0093] Among the curable compounds, polyfunctional acrylates or polyfunctional methacrylates are preferred from the viewpoint of curability.
[0094] Among these, polyfunctional methacrylates are particularly preferred from the viewpoint of high resistance to acidic gases and the like and the ability to suppress image deletion even after repeated printing. It has been confirmed that polyfunctional methacrylates have higher resistance to acidic gases and the like than polyfunctional acrylates. Therefore, when polyfunctional acrylates are used as the curable resin for the protective layer, they tend to deteriorate due to acidic gases generated from chargers and the like over the course of repeated printing, resulting in image deletion. However, when polyfunctional methacrylates are used, the occurrence of image deletion can be suppressed even after repeated printing.
[0095] Examples of polyfunctional acrylates include urethane acrylate, alkyl acrylate, hydroxyl group-containing alkyl acrylate, polyethylene glycol acrylate, polypropylene glycol acrylate, polytetramethylene glycol acrylate, dioxane acrylate, tricyclodecanol acrylate, fluorene acrylate, alkoxylated bisphenol A acrylate, (alkoxylated) trimethylolpropane acrylate, (alkoxylated) ditrimethylolpropane acrylate, (alkoxylated) glycerin acrylate, (caprolactone-modified) isocyanurate acrylate, (alkoxylated) pentaerythritol acrylate, (alkoxylated) ditrimethylolpropane methacrylate, (alkoxylated) dipentaerythritol methacrylate, polypentaerythritol polyacrylate, and dendritic polymer acrylate. Among these, urethane acrylate, (alkoxylated) trimethylolpropane acrylate, (alkoxylated) ditrimethylolpropane acrylate, (alkoxylated) pentaerythritol acrylate, and (alkoxylated) dipentaerythritol acrylate are preferred, and urethane acrylate, (alkoxylated) ditrimethylolpropane acrylate, and (alkoxylated) pentaerythritol acrylate are more preferred.
[0096] Examples of polyfunctional methacrylates include urethane methacrylate, alkyl methacrylate, hydroxyl group-containing methacrylate, polyethylene glycol methacrylate, polypropylene glycol methacrylate, tricyclodecanol methacrylate, ethoxylated bisphenol A methacrylate, (alkoxylated) trimethylolpropane methacrylate, (alkoxylated) ditrimethylolpropane methacrylate, ethoxylated glycerin methacrylate, (alkoxylated) pentaerythritol methacrylate, (alkoxylated) ditrimethylolpropane methacrylate, and (alkoxylated) dipentaerythritol methacrylate. Among these, urethane methacrylate, (alkoxylated) trimethylolpropane methacrylate, (alkoxylated) ditrimethylolpropane methacrylate, (alkoxylated) pentaerythritol methacrylate, and (alkoxylated) dipentaerythritol methacrylate are preferred, and urethane methacrylate, (alkoxylated) trimethylolpropane methacrylate, and (alkoxylated) ditrimethylolpropane methacrylate are more preferred.
[0097] The number of functional groups of the polyfunctional methacrylate is preferably 2 or more from the viewpoint of hardness, and more preferably 3 or more from the viewpoint of elastic deformation rate, while it is preferably 10 or less, and more preferably 6 or less from the viewpoint of curing degree, and more preferably 4 or less from the viewpoint of curing degree.
[0098] When the protective layer contains metal oxide particles, the content of the metal oxide particles relative to 100 parts by mass of the curable compound is preferably 20 parts by mass or more, more preferably 60 parts by mass or more, and is preferably 500 parts by mass or less, more preferably 200 parts by mass or less, from the viewpoint of electrical properties.
[0099] [Solvent Used in Coating Liquid for Forming Protective Layer] Examples of organic solvents used in the coating liquid for forming the protective layer include alcohols such as methanol, ethanol, propanol, and 2-methoxyethanol; ethers such as tetrahydrofuran, 1,4-dioxane, and dimethoxyethane; esters such as methyl formate and ethyl acetate; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; aromatic hydrocarbons such as benzene, toluene, xylene, and anisole; chlorinated hydrocarbons such as dichloromethane, chloroform, 1,2-dichloroethane, 1,1,2-trichloroethane, 1,1,1-trichloroethane, tetrachloroethane, 1,2-dichloropropane, and trichloroethylene; nitrogen-containing compounds such as n-butylamine, isopropanolamine, diethylamine, triethanolamine, ethylenediamine, and triethylenediamine; and aprotic polar solvents such as acetonitrile, N-methylpyrrolidone, N,N-dimethylformamide, and dimethyl sulfoxide. Mixed solvents of these solvents may also be used in any combination and in any ratio. Furthermore, even if an organic solvent does not dissolve the material for the protective layer of the electrophotographic photoreceptor by itself, it can be used if it can dissolve the material by, for example, mixing it with the above-mentioned organic solvent. Generally, using a mixed solvent can reduce coating unevenness. When using a dip coating method as the coating method described below, it is preferable to select a solvent that does not dissolve the lower layer. From this perspective, it is preferable to contain alcohols that have low solubility in polycarbonate and polyarylate, which are suitable for use in the photosensitive layer.
[0100] The ratio of the amount of the organic solvent to the amount of the solid content used in the coating solution for forming the protective layer varies depending on the coating method for the coating solution for forming the protective layer, and may be appropriately changed so as to form a uniform coating film in the coating method to be used.
[0101] [Content in the Protective Layer-Forming Coating Liquid] The blending ratio of the compound having the structure represented by Formula (3) or Formula (4) relative to the curable compound is preferably 0.1 parts by mass or more and 15 parts by mass or less per 100 parts by mass of the curable compound. It is preferable that the blending ratio of the compound having the structure represented by Formula (3) or Formula (4) is 0.1 parts by mass or more per 100 parts by mass of the curable compound, from the viewpoint of promoting curing of the protective layer. From this viewpoint, it is more preferable that the blending ratio of the compound having the structure represented by Formula (3) or Formula (4) is 0.3 parts by mass or more, more preferably 1 part by mass or more, and even more preferably 3 parts by mass or more. On the other hand, it is preferable that the blending ratio of the compound having the structure represented by Formula (3) or Formula (4) is 15 parts by mass or less per 100 parts by mass of the curable compound, from the viewpoint of electrical measurement. From this viewpoint, it is more preferable that the blending ratio of the compound represented by Formula (3) or Formula (4) is 10 parts by mass or less, more preferably 8 parts by mass or less, and even more preferably 6 parts by mass or less.
[0102] When metal oxide particles are blended into the protective layer-forming coating liquid, the blending ratio of the compound having the structure represented by formula (3) or (4) is preferably 0.3 parts by mass or more and 15 parts by mass or less relative to 100 parts by mass of the metal oxide particles. It is preferable that the blending ratio of the compound having the structure represented by formula (3) or (4) is 0.3 parts by mass or more relative to 100 parts by mass of the metal oxide particles, from the viewpoint of promoting curing of the protective layer. From this viewpoint, it is more preferable that the blending ratio of the compound having the structure represented by formula (3) or (4) is 1 part by mass or more, more preferably 2 parts by mass or more, and even more preferably 3 parts by mass or more. On the other hand, it is preferable that the blending ratio of the compound having the structure represented by formula (3) or (4) is 15 parts by mass or less relative to 100 parts by mass of the metal oxide particles, from the viewpoint of suppressing aggregation of the metal oxide particles. From this viewpoint, it is more preferable that the blending ratio of the compound represented by formula (3) or (4) is 10 parts by mass or less, more preferably 8 parts by mass or less, and even more preferably 6 parts by mass or less.
[0103] [Coating Method] The method for applying the coating solution for forming the protective layer is not particularly limited, and examples thereof include spray coating, spiral coating, ring coating, and dip coating.
[0104] After forming the coating film by the above coating method, the coating film is dried. In this case, the drying temperature and time are not important as long as necessary and sufficient drying is obtained. However, if the protective layer is coated by only air drying after coating the photosensitive layer, it is preferable to carry out sufficient drying by the method described below in the method for forming the photosensitive layer.
[0105] [Method for Curing the Protective Layer] The protective layer can be formed by applying the protective layer-forming coating liquid and then curing it by applying external energy. Examples of the external energy used in this process include heat, light, and radiation.
[0106] Examples of methods for applying heat energy include heating methods using gases such as air and nitrogen, steam, various heat transfer media, infrared rays, and electromagnetic waves. Heating can be carried out from the coated surface side or the support side. The heating temperature is preferably 100°C or higher and 170°C or lower.
[0107] As the light energy, UV irradiation light sources such as high-pressure mercury lamps, metal halide lamps, electrodeless lamp bulbs, and light-emitting diodes, which have emission wavelengths mainly in the ultraviolet (UV) range, can be used. It is also possible to select a visible light source in accordance with the absorption wavelengths of the chain polymerizable compound and the photopolymerization initiator. The light irradiation dose is set to 10 J / cm from the viewpoint of curing properties. 2 More than 30 J / cm is preferable. 2 More preferably, 100 J / cm or more 2 In addition, from the viewpoint of electrical properties, 500 J / cm or more is particularly preferable. 2 Preferably, 300 J / cm or less 2 More preferably, 200 J / cm or less 2 The following are particularly preferred: On the other hand, examples of radiation energy include those using electron beams (EB).
[0108] Among these energies, light energy is preferred from the viewpoints of ease of reaction rate control, simplicity of the device, and long pod life.
[0109] After the protective layer is cured, a heating step may be performed from the viewpoints of relieving residual stress, relieving residual radicals, and improving electrical properties. The heating temperature is preferably 60° C. or higher, more preferably 100° C. or higher, and is preferably 200° C. or lower, more preferably 150° C. or lower.
[0110] (Layer Thickness) From the viewpoint of abrasion resistance, the thickness of the protective layer is preferably 0.5 μm or more, more preferably 1 μm or more. On the other hand, from the viewpoint of electrical properties, it is preferably 5 μm or less, more preferably 3 μm or less. From the same viewpoint, the thickness of the protective layer is preferably 1 / 50 or more of the thickness of the photosensitive layer, more preferably 1 / 40 or more, and even more preferably 1 / 30 or more. On the other hand, it is preferably 1 / 3 or less, more preferably 1 / 5 or less, and even more preferably 1 / 10 or less.
[0111] <Photosensitive Layer> The photosensitive layer in the electrophotographic photoreceptor (also referred to as "photosensitive layer") may be any layer containing at least a charge generating material (CGM) and a charge transport material.
[0112] The photosensitive layer may be a single-layer type photosensitive layer containing both a charge generating material and a charge transporting material in the same layer, or may be a multi-layer type photosensitive layer separated into a charge generating layer and a charge transporting layer.
[0113] <Single-Layer Photosensitive Layer> When the photosensitive layer is a single-layer photosensitive layer, it is preferable that at least a charge generating material (CGM), a hole transporting material (HTM), an electron transporting material (ETM), and a binder resin are contained in the same layer.
[0114] (Charge-Generating Material) As the charge-generating material used in the photosensitive layer, various photoconductive materials such as inorganic photoconductive materials and organic pigments can be used. Among them, organic pigments are particularly preferred, and phthalocyanine pigments and azo pigments are more preferred.
[0115] In particular, when a phthalocyanine pigment is used as the charge generating material, specifically, metal-free phthalocyanine, phthalocyanine coordinated with a metal such as copper, indium, gallium, tin, titanium, zinc, vanadium, silicon, or germanium, or an oxide or halide thereof, is used. Examples of ligands to trivalent or higher metal atoms include the oxygen atom and chlorine atom listed above, as well as a hydroxy group and an alkoxy group. Among these, particularly highly sensitive X-type and τ-type metal-free phthalocyanine, A-type, B-type, D-type titanyl phthalocyanine, vanadyl phthalocyanine, chloroindium phthalocyanine, chlorogallium phthalocyanine, hydroxygallium phthalocyanine, and the like are preferred.
[0116] When an azo pigment is used, various known bisazo pigments and trisazo pigments are preferably used.
[0117] The charge generation substance may be used alone or in any combination and ratio of two or more. When two or more charge generation substances are used in combination, the charge generation substances may be mixed after the respective charge generation substances are mixed, or may be mixed during the production or processing steps of the charge generation substances, such as synthesis, pigmentation, or crystallization.
[0118] From the viewpoint of electrical properties, it is desirable that the particle diameter of the charge generating material is small. Specifically, the particle diameter of the charge generating material is preferably 1 μm or less, more preferably 0.5 μm or less. The lower limit is 0.01 μm or more. Here, the particle diameter of the charge generating material means the particle diameter in a state in which it is contained in the photosensitive layer.
[0119] Furthermore, the amount of the charge generating substance in the single-layer photosensitive layer is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, from the viewpoint of sensitivity, and is preferably 50% by mass or less, more preferably 20% by mass or less, from the viewpoint of sensitivity and chargeability.
[0120] (Charge transport material) Charge transport materials are classified into hole transport materials having mainly hole transport ability and electron transport materials having mainly electron transport ability. However, when the present photosensitive layer is a single-layer type photosensitive layer, it is preferable that at least a hole transport material and an electron transport material are contained in the same layer.
[0121] [Hole Transport Material] The hole transport material (HTM) can be selected from known materials and used. Examples include electron donating materials such as heterocyclic compounds such as carbazole derivatives, indole derivatives, imidazole derivatives, oxazole derivatives, pyrazole derivatives, thiadiazole derivatives, and benzofuran derivatives, aniline derivatives, hydrazone derivatives, arylamine derivatives, stilbene derivatives, butadiene derivatives, and enamine derivatives, as well as compounds in which a plurality of these compounds are bonded, and polymers having groups consisting of these compounds in the main chain or side chain.
[0122] Among these, carbazole derivatives, arylamine derivatives, stilbene derivatives, butadiene derivatives, enamine derivatives, and compounds in which a plurality of these compounds are combined are preferred, and arylamine derivatives and enamine derivatives are more preferred.
[0123] From the viewpoint of electrical properties, the molecular weight of the hole transport substance is preferably 600 or more, more preferably 650 or more, even more preferably 700 or more, and particularly preferably 740 or more. On the other hand, from the viewpoint of ease of synthesis and stability of the compound, the molecular weight is preferably 1200 or less, more preferably 1000 or less, and even more preferably 900 or less.
[0124] The hole transporting substance may be used alone or in any combination of two or more kinds in any ratio.
[0125] Preferred examples of the structure of the hole transport material are shown below.
[0126]
[0127]
[0128]
[0129] Among the above hole transport materials, HTM31, HTM32, HTM33, HTM34, HTM35, HTM39, HTM40, HTM41, HTM42, HTM43, and HTM48 are preferred from the viewpoint of electrical properties, and HTM39, HTM40, HTM41, HTM42, HTM43, and HTM48 are more preferred.
[0130] [Electron Transporting Material] The electron transporting material (ETM) can be selected from known materials. Examples include electron-withdrawing substances such as aromatic nitro compounds such as 2,4,7-trinitrofluorenone, cyano compounds such as tetracyanoquinodimethane, and quinone compounds such as diphenoquinone, as well as known cyclic ketone compounds and perylene pigments (perylene derivatives). Among these, from the viewpoint of electrical properties, quinone compounds and perylene pigments (perylene derivatives) are preferred, and quinone compounds are more preferred. Among the quinone compounds, from the viewpoint of electrical properties, diphenoquinone or dinaphthylquinone is preferred. Of these, dinaphthylquinone is more preferred.
[0131] From the viewpoint of electrical properties, the molecular weight of the electron transport material is preferably 400 or more, more preferably 410 or more, and even more preferably 420 or more, and is preferably 1000 or less, more preferably 800 or less, and even more preferably 600 or less.
[0132] The electron transport material may be used alone or in any combination of two or more kinds in any ratio.
[0133] Preferred examples of the structure of the electron transport material are shown below.
[0134]
[0135] Among the above electron transport materials, ET-2 and ET-5 are preferred, with ET-2 being more preferred, in terms of electrical properties.
[0136] [Contents of Hole Transport Substance and Electron Transport Substance] The ratio of the mass of the electron transport substance to the mass of the hole transport substance in the single-layer photosensitive layer is preferably 0.3 or more from the viewpoint of electron transportability, and more preferably 0.4 or more from the viewpoint of electrical properties. On the other hand, from the viewpoint of hole transportability, it is preferably 1.0 or less, and more preferably 0.9 or less from the viewpoint of suppressing precipitation of the electron transport substance, and more preferably 0.8 or less from the viewpoint of adhesion.
[0137] From the viewpoint of hole transportability, the content of the hole transport substance in the electrophotographic photoreceptor is preferably 50 parts by mass or more, more preferably 80 parts by mass or more, and even more preferably 90 parts by mass or more, relative to 100 parts by mass of the binder resin described below. On the other hand, from the viewpoint of suppressing precipitation, the upper limit is more preferably 200 parts by mass or less, and even more preferably 150 parts by mass or less.
[0138] (Binder Resin) Next, the binder resin used in the present photosensitive layer will be described. Examples of binder resins used in the present photosensitive layer include vinyl polymers or copolymers thereof such as polymethyl methacrylate, polystyrene, and polyvinyl chloride; vinyl alcohol resins; polyvinyl butyral resins; polyvinyl formal resins; partially modified polyvinyl acetal resins; polyarylate resins; polyamide resins; polyurethane resins; polycarbonate resins; polyester resins; polyester carbonate resins; polyimide resins; phenoxy resins; epoxy resins; silicone resins; and partially crosslinked cured products thereof. The above resins may also be modified with a silicon reagent or the like. These may be used alone or in any combination and ratio.
[0139] The binder resin used in the present photosensitive layer preferably contains one or more polymers obtained by interfacial polymerization.
[0140] The binder resin obtained by the interfacial polymerization is preferably a polycarbonate resin or a polyester resin, more preferably a polycarbonate resin or a polyarylate resin, and particularly preferably a polymer made from an aromatic diol.
[0141] (Other Substances) In addition to the materials described above, the photosensitive layer may contain additives such as well-known antioxidants, plasticizers, ultraviolet absorbers, electron-withdrawing compounds, leveling agents, and visible light shielding agents in order to improve film-forming properties, flexibility, coating properties, contamination resistance, gas resistance, light resistance, and the like. The photosensitive layer may also contain various additives, such as sensitizers, dyes, pigments (excluding the charge-generating materials, hole-transporting materials, and electron-transporting materials described above), and surfactants, as needed. Examples of surfactants include silicone oils and fluorine-based compounds. In the present invention, these may be used alone or in any combination and ratio.
[0142] Furthermore, for the purpose of reducing frictional resistance on the surface of the photosensitive layer, the photosensitive layer may contain a fluorine-based resin, a silicone resin, or the like, or may contain particles made of these resins or particles of an inorganic compound such as aluminum oxide.
[0143] (Layer Thickness) When the present photosensitive layer is a single-layer type photosensitive layer, the thickness of the present photosensitive layer is preferably 20 μm or more, more preferably 25 μm or more, from the viewpoint of dielectric breakdown resistance, and is preferably 50 μm or less, more preferably 40 μm or less, from the viewpoint of electrical properties.
[0144] <Laminated Photosensitive Layer> When the present electrophotographic photoreceptor is a laminated photosensitive layer, for example, a configuration in which a charge transport layer (CTL) containing an electron transport material (ETM) and a hole transport material (HTM) is laminated on a charge generation layer (CGL) containing a charge generation material (CGM) can be mentioned. In this case, it is also possible to provide layers other than the charge generation layer (CGL) and the charge transport layer (CTL).
[0145] <Charge Generation Layer (CGL)> The charge generation layer usually contains a charge generation material (CGM) and a binder resin. The charge generation material (CGM) and the binder resin are the same as those described above for the single-layer photosensitive layer.
[0146] (Other Components) In addition to the charge generating material and the binder resin, the charge generating layer may contain other components as needed. For example, known additives such as antioxidants, plasticizers, ultraviolet absorbers, electron-withdrawing compounds, leveling agents, visible light shielding agents, and fillers may be contained in order to improve film-forming properties, flexibility, coating properties, contamination resistance, gas resistance, light resistance, etc.
[0147] (Composition ratio) In the charge generation layer, if the ratio of the charge generation material is too high, the stability of the coating liquid may decrease due to aggregation of the charge generation material, etc., while if the ratio of the charge generation material is too low, the sensitivity of the photoreceptor may decrease. Therefore, the composition ratio (by mass) of the binder resin to the charge generation material is preferably 10 parts by mass or more of the charge generation material per 100 parts by mass of the binder resin, and more preferably 30 parts by mass or more. On the other hand, it is preferably 1,000 parts by mass or less, and more preferably 500 parts by mass or less. From the viewpoint of film strength, it is more preferably 300 parts by mass or less, and even more preferably 200 parts by mass or less.
[0148] (Layer Thickness) The thickness of the charge generating layer is preferably 0.1 μm or more, more preferably 0.15 μm or more, and is preferably 10 μm or less, more preferably 0.6 μm or less.
[0149] <Charge Transport Layer (CTL)> The charge transport layer (CTL) usually contains a hole transport material (HTM) and a binder resin, and may further contain an electron transport material (ETM). The electron transport material (ETM), hole transport material (HTM), and binder resin are the same as those described in the single-layer type photosensitive layer above.
[0150] In the charge transport layer (CTL), the blending ratio of the binder resin and the hole transport material (HTM) is preferably 20 parts by mass or more of the hole transport material (HTM) per 100 parts by mass of the binder resin, more preferably 30 parts by mass or more from the viewpoint of reducing residual potential, and even more preferably 40 parts by mass or more from the viewpoints of stability during repeated use and charge mobility. On the other hand, from the viewpoint of thermal stability of the photosensitive layer, the blending ratio of the hole transport material (HTM) per 100 parts by mass of the binder resin is preferably 200 parts by mass or less, and from the viewpoint of compatibility between the hole transport material (HTM) and the binder resin, more preferably 150 parts by mass or less, and particularly preferably 120 parts by mass or less from the viewpoint of glass transition temperature.
[0151] (Other Components) The charge transport layer may contain other components as needed in addition to the electron transport material (ETM), hole transport material (HTM), and binder resin. For example, known additives such as antioxidants, plasticizers, ultraviolet absorbers, electron-withdrawing compounds, leveling agents, visible light shielding agents, and fillers may be contained for the purpose of improving film-forming properties, flexibility, coatability, contamination resistance, gas resistance, light resistance, etc.
[0152] (Layer Thickness) The layer thickness of the charge transport layer is not particularly limited. From the viewpoints of electrical characteristics, image stability, and high resolution, the layer thickness is preferably 5 μm or more and 50 μm or less, more preferably 10 μm or more or 35 μm or less, and even more preferably 15 μm or more or 25 μm or less.
[0153] <Method of Forming Photosensitive Layer> In both the multilayer type and the single-layer type, each of the above layers can be formed as follows. A coating liquid obtained by dissolving or dispersing a substance to be contained in a solvent can be applied to a conductive support by a known method such as dip coating, spray coating, nozzle coating, bar coating, roll coating, or blade coating, and the layers can be formed by repeating the steps of coating and drying sequentially for each layer. However, the formation method is not limited to this.
[0154] The solvent or dispersion medium used in preparing the coating liquid is not particularly limited. Specific examples include alcohols such as methanol, ethanol, propanol, and 2-methoxyethanol; ethers such as tetrahydrofuran, 1,4-dioxane, and dimethoxyethane; aromatic hydrocarbons such as benzene, toluene, and xylene; and chlorinated hydrocarbons such as dichloromethane, chloroform, 1,2-dichloroethane, 1,1,2-trichloroethane, 1,1,1-trichloroethane, tetrachloroethane, 1,2-dichloropropane, and trichloroethylene. These solvents may be used alone, or two or more may be used in any combination and type.
[0155] The amount of solvent or dispersion medium used is not particularly limited. It is preferable to appropriately adjust the solids concentration, viscosity, and other physical properties of the coating solution so that they fall within the desired range, taking into account the purpose of each layer and the properties of the selected solvent or dispersion medium. The coating film is preferably dried by heating, usually at a temperature of 30°C or higher and 200°C or lower, for 1 minute to 2 hours, either stationary or under airflow. The heating temperature may be constant, or the temperature may be varied during drying.
[0156] <Conductive Support> The conductive support (also referred to as the "conductive support") of the electrophotographic photoreceptor is not particularly limited as long as it supports a layer formed thereon and exhibits electrical conductivity. Examples of the conductive support include metal materials such as aluminum, aluminum alloys, stainless steel, copper, and nickel, resin materials imparted with electrical conductivity by the coexistence of metals, carbon, and conductive powders such as tin oxide, and resins, glass, and paper on whose surfaces conductive materials such as aluminum, nickel, and ITO (indium oxide tin oxide alloy) are vapor-deposited or coated. The conductive support may be in the form of a drum, cylinder, sheet, belt, or the like. The conductive support may be a metal conductive support coated with a conductive material having an appropriate resistance value for controlling electrical conductivity, surface properties, and the like or for covering defects.
[0157] When a metal material such as an aluminum alloy is used as the conductive support, the metal material may be anodized before use.
[0158] The average thickness of the anodic oxide coating is preferably 20 μm or less, and more preferably 7 μm or less.
[0159] When forming an anodized film on a metal material, it is preferable to perform a sealing treatment. The sealing treatment can be performed by a known method.
[0160] The surface of the conductive support may be smooth or may be roughened by using a special cutting method or by polishing. Alternatively, the surface may be roughened by mixing particles of an appropriate particle size into the material constituting the support. An undercoat layer, which will be described below, may be provided between the conductive support and the photosensitive layer to improve adhesion, blocking resistance, etc.
[0161] <Present Undercoat Layer> The present electrophotographic photoreceptor may have an undercoat layer (also referred to as "present undercoat layer") between the present photosensitive layer and the present conductive support.
[0162] The undercoat layer can be made of, for example, a resin, or a resin in which organic pigments or particles of metal oxides or the like are dispersed. Examples of organic pigments used in the undercoat layer include phthalocyanine pigments, azo pigments, and perylene pigments. Among these, phthalocyanine pigments and azo pigments, specifically, the phthalocyanine pigments and azo pigments used as the charge generating material described above, can be mentioned.
[0163] Examples of metal oxide particles used in the present undercoat layer include metal oxide particles containing one type of metal element such as titanium oxide, aluminum oxide, silicon oxide, zirconium oxide, zinc oxide, and iron oxide, and metal oxide particles containing multiple metal elements such as calcium titanate, strontium titanate, and barium titanate. The undercoat layer may contain only one type of particle, or multiple types of particles may be mixed in any ratio and combination.
[0164] Among the above metal oxide particles, titanium oxide and aluminum oxide are preferred, and titanium oxide is particularly preferred. The titanium oxide particles may have their surfaces treated with any inorganic or organic substance. The titanium oxide particles may be in any of the following crystal forms: rutile, anatase, brookite, and amorphous. Titanium oxide particles may also be in a variety of crystal forms.
[0165] The particle size of the metal oxide particles used in the present undercoat layer is not particularly limited. From the viewpoints of the properties of the undercoat layer and the stability of the solution for forming the undercoat layer, the average primary particle size is preferably 10 nm or more, and 100 nm or less, more preferably 50 nm or less.
[0166] The binder resin used in the undercoat layer may be selected from, for example, polyvinyl acetal-based resins such as polyvinyl butyral resins, polyvinyl formal resins, and partially acetalized polyvinyl butyral resins in which a portion of butyral is modified with formal or acetal; and insulating resins such as polyarylate resins, polycarbonate resins, polyester resins, phenoxy resins, acrylic resins, methacrylic resins, polyamide resins, polyurethane resins, epoxy resins, silicone resins, polyvinyl alcohol resins, styrene-alkyd resins, silicone-alkyd resins, and phenol-formaldehyde resins. However, the binder resin is not limited to these polymers. These binder resins may be used alone or in combination, or may be used in a cured form with a curing agent. Among these, polyvinyl acetal-based resins, alcohol-soluble copolymer polyamides, modified polyamides, and the like are preferred due to their excellent dispersibility and coatability. Of these, alcohol-soluble copolymer polyamides are particularly preferred.
[0167] The mixing ratio of the particles to the binder resin can be selected arbitrarily, but it is preferable to use the particles in the range of 10% by mass to 500% by mass in terms of the stability and coatability of the dispersion.
[0168] The thickness of the undercoat layer can be selected arbitrarily. In view of the characteristics of the electrophotographic photoreceptor and the coating properties of the dispersion, the thickness is preferably 0.1 μm or more, and more preferably 20 μm or less. The undercoat layer may also contain a known antioxidant.
[0169] <Other Layers> The electrophotographic photoreceptor may have other layers as needed, in addition to the conductive support, photosensitive layer, protective layer, and undercoat layer described above.
[0170] <Physical Properties of the Electrophotographic Photoreceptor> The electrophotographic photoreceptor can have the following physical properties.
[0171] (Martens Hardness) In order to provide the electrophotographic photoreceptor with sufficient wear resistance for practical use, the Martens hardness is set to 170 N / mm 2 More preferably, it is 200 N / mm 2 Above all, 250N / mm 2 Above all, 300N / mm 2 In the present invention, the Martens hardness of the photoreceptor means the Martens hardness measured from the surface side of the photoreceptor. The Martens hardness can be measured by the method described in the examples below.
[0172] (Elastic Deformation Rate) From the viewpoint of providing practically sufficient wear resistance, the electrophotographic photosensitive member preferably has an elastic deformation rate of 25% or more, more preferably 30% or more, even more preferably 35% or more, and particularly preferably 40% or more. In the present invention, the elastic deformation rate of the photosensitive member means the elastic deformation rate measured from the surface side of the photosensitive member. The elastic deformation rate can be measured by the method described in the Examples below.
[0173] <<Present Image Forming Apparatus>> An image forming apparatus ("present image forming apparatus") can be configured using the present electrophotographic photoreceptor.
[0174] As shown in Figure 1, the image forming apparatus is configured to include an electrophotographic photoreceptor 1, a charging device 2, an exposure device 3, and a developing device 4, and may further include a transfer device 5, a cleaning device 6, and a fixing device 7 as needed. There are no particular limitations on the electrophotographic photoreceptor 1 as long as it is the electrophotographic photoreceptor described above. Figure 1 shows, as an example, a drum-shaped photoreceptor in which the above-described photosensitive layer is formed on the surface of a cylindrical conductive support. The charging device 2, exposure device 3, developing device 4, transfer device 5, and cleaning device 6 are arranged along the outer circumferential surface of the electrophotographic photoreceptor 1, respectively.
[0175] Examples of the charging device 2 include a non-contact corona charging device such as a corotron or scorotron, or a contact-type charging device (direct-type charging device) that charges the photosensitive member by bringing a charging member to which a voltage is applied into contact with the surface of the photosensitive member. Examples of contact charging devices include a charging roller and a charging brush. Note that FIG. 1 shows a roller-type charging device (charging roller) as an example of the charging device 2.
[0176] The type of exposure device 3 is not particularly limited as long as it can expose the electrophotographic photoreceptor 1 to light and form an electrostatic latent image on the photosensitive surface of the electrophotographic photoreceptor 1. Furthermore, exposure may be performed by an internal photoreceptor exposure method. Any light may be used for exposure.
[0177] The type of toner T is arbitrary, and in addition to powder toner, polymerized toner produced by a suspension polymerization method or an emulsion polymerization method can be used.
[0178] The developing device 4 may have any configuration. The developing device 4 shown in Fig. 1 has a configuration in which the toner T is formed into a thin layer by a regulating member (developing blade) 45, frictionally charged to a predetermined polarity, and carried and transported by a developing roller 44 to contact the surface of the photoreceptor 1. However, this configuration is not limited to this. The transfer device 5 is not particularly limited in type, and any device using an electrostatic transfer method such as corona transfer, roller transfer, or belt transfer, a pressure transfer method, or an adhesive transfer method may be used.
[0179] There are no particular limitations on the cleaning device 6. Any cleaning device, such as a brush cleaner or blade cleaner, can be used. If there is little or almost no toner remaining on the photoreceptor surface, the cleaning device 6 may be omitted. The fixing device 7 may also have any configuration. In addition to the configuration described above, the image forming apparatus may also be configured to be capable of performing, for example, a static elimination process.
[0180] Furthermore, the image forming apparatus may be further modified and configured, for example, to be capable of performing processes such as a pre-exposure process and an auxiliary charging process, or to be configured to perform offset printing, or even to be configured as a full-color tandem system using multiple types of toner.
[0181] <<Present Electrophotographic Cartridge>> The present electrophotographic photosensitive member 1 can be combined with one or more of the charging device 2, the exposure device 3, the developing device 4, the transfer device 5, the cleaning device 6, and the fixing device 7 to form an integrated cartridge (referred to as the present electrophotographic cartridge). However, the present electrophotographic cartridge described below is one example of an electrophotographic cartridge that can be formed using the present electrophotographic photosensitive member, and is not limited to the present electrophotographic cartridge.
[0182] The electrophotographic cartridge can be configured to be detachable from the main body of an electrophotographic apparatus such as a copying machine, a laser beam printer, etc. In this case, for example, when the electrophotographic photosensitive member 1 or other members deteriorate, the electrophotographic photosensitive member cartridge can be removed from the main body of the image forming apparatus and a new electrophotographic photosensitive member cartridge can be mounted in the main body of the image forming apparatus, thereby facilitating maintenance and management of the image forming apparatus.
[0183] <<Explanation of Terms>> In the present invention, when "X to Y" (X and Y are any numbers) is expressed, unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably larger than X" or "preferably smaller than Y". Furthermore, when "X or more" (X is any number) or "Y or less" (Y is any number) is expressed, it also includes the meaning of "preferably larger than X" or "preferably smaller than Y".
[0184] Hereinafter, the embodiments of the present invention will be described in more detail with reference to examples. However, the following examples are provided to explain the present invention in detail, and the present invention is not limited to the examples shown below, and can be practiced by modifying it as desired, as long as it does not deviate from the gist of the present invention. Furthermore, in the following examples and comparative examples, "parts" refers to "parts by mass" unless otherwise specified.
[0185] (Preparation of Coating Solution P1 for Forming Undercoat Layer) 20 parts of D-type titanyl phthalocyanine, which exhibits a clear peak at a diffraction angle 2θ=27.3°±0.2° in powder X-ray diffraction using CuKα radiation, and 280 parts of 1,2-dimethoxyethane were mixed and pulverized for 2 hours in a sand grind mill to perform a fine particle dispersion treatment. 400 parts of a 2.5% 1,2-dimethoxyethane solution of polyvinyl butyral (manufactured by Denki Kagaku Kogyo Co., Ltd., trade name "Denka Butyral" #6000C) and 170 parts of 1,2-dimethoxyethane were further added and mixed to prepare Coating Solution P1 for forming undercoat layer.
[0186] (Preparation of Coating Solution Q1 for Forming Single-Layer Photosensitive Layer) A single-layer photosensitive layer-forming coating solution Q1 having a solids concentration of 25% by mass was prepared by mixing 2.6 parts of D-type titanyl phthalocyanine that exhibits a clear peak at a diffraction angle 2θ=27.3°±0.2° in powder X-ray diffraction using CuKα radiation, 1.3 parts of perylene pigment 1 having the structure shown below, 0.5 parts of polyvinyl butyral resin, 100 parts of the hole transport material shown below (HTM48, molecular weight 748), 60 parts of the electron transport material shown below (ET-2, molecular weight 424.2), 100 parts of a polycarbonate resin having a biphenyl structure, 0.05 parts of silicone oil (manufactured by Shin-Etsu Silicones Co., Ltd.: trade name KF-96) as a leveling agent, and 793.35 parts of a mixed solvent of tetrahydrofuran (hereinafter appropriately abbreviated as THF) and toluene (hereinafter appropriately abbreviated as TL) (THF 80% by mass, TL 20% by mass).
[0187]
[0188]
[0189]
[0190] (Preparation of Coating Solution S1 for Forming Protective Layer) A curable compound M-1 (manufactured by Shin-Nakamura Chemical Co., Ltd., product name TMPT) represented by the structure below, which had been dissolved in advance in a mixed solvent of methanol / 1-propanol / toluene, a compound O-1 represented by the structure below as a polymerization initiator, and a dispersed slurry of titanium oxide particles (average primary particle size 40 nm, surface-treated with 3.5 wt % methyldimethoxysilane) were mixed to obtain a coating solution S1 for forming a protective layer (solid concentration 30 mass %) in which the ratio of M-1 / titanium oxide particles / O-1 was 100 / 100 / 3 (mass ratio) and the solvent composition was methanol / 1-propanol / toluene = 7 / 1 / 2 (mass ratio).
[0191] [M-1]
[0192] [O-1]
[0193] O-1 is a compound represented by the above formulas (3) and (4), and R 1 has the following structure: where W represents the bond to the carbon to which R is bonded.
[0194]
[0195] (Preparation of protective layer forming coating solution S2) A protective layer forming coating solution S2 was prepared in the same manner as the protective layer forming coating solution S1, except that the polymerization initiator O-1 was changed to a polymerization initiator O-2 represented by the following structure.
[0196] [O-2]
[0197] O-2 is a compound represented by the above formulas (3) and (4), and R 1 has the following structure: where W represents the bond to the carbon to which R is bonded.
[0198]
[0199] (Preparation of protective layer forming coating solution S3) A protective layer forming coating solution S3 was prepared in the same manner as the protective layer forming coating solution S1, except that the polymerization initiator O-1 was changed to a polymerization initiator O-3 represented by the following structure.
[0200] [O-3]
[0201] O-3 is a compound represented by the above formulas (3) and (4), and R 1 has the following structure: where W represents the bond to the carbon to which R is bonded.
[0202]
[0203] (Preparation of protective layer-forming coating liquid S4) A protective layer-forming coating liquid S4 was prepared in the same manner as the protective layer-forming coating liquid S1, except that the curable compound M-1 was changed to a curable compound M-2 (manufactured by Shin-Nakamura Chemical Co., Ltd., product name M-DPH-6E) represented by the following structure.
[0204] [M-2] [Formula (19)]
[0205] In formula (19), each R is —O—CH 2 -CH 2 -, f+g+h+i+j+k=6, Q is a hydroxy group or the following formula (20), Z 1 are all methyl groups.
[0206] [Formula (20)]
[0207] In formula (20), Z 2 represents a bond to R in formula (19). 1 represents a methyl group.
[0208] (Preparation of Coating Solution S5 for Forming Protective Layer) Coating Solution S5 for forming protective layer was prepared in the same manner as Coating Solution S4 for Forming Protective Layer, except that the polymerization initiator O-1 was changed to polymerization initiator O-3 and the contents were changed to the following ratio: M-DPH-6E / titanium oxide particles / O-3=100 / 100 / 6 (mass ratio).
[0209] (Preparation of Coating Solution S6 for Forming Protective Layer) Coating Solution S6 for forming protective layer was prepared in the same manner as Coating Solution S4 for Forming Protective Layer, except that the polymerization initiator O-1 was changed to Polymerization Initiator O-3 and the contents were changed to the following ratio: M-DPH-6E / Titanium oxide particles / O-3=100 / 100 / 3 (mass ratio).
[0210] (Preparation of Coating Solution S7 for Forming Protective Layer) Coating Solution S7 for forming protective layer was prepared in the same manner as Coating Solution S4 for Forming Protective Layer, except that the polymerization initiator O-1 was changed to polymerization initiator O-3 and the contents were changed to the following ratio: M-DPH-6E / titanium oxide particles / O-3 = 100 / 100 / 1 (mass ratio).
[0211] (Preparation of Coating Solution S8 for Forming Protective Layer) Coating Solution S8 for forming protective layer was prepared in the same manner as Coating Solution S4 for Forming Protective Layer, except that the polymerization initiator O-1 was changed to Polymerization Initiator O-3 and the contents were changed to the following ratio: M-DPH-6E / Titanium Oxide Particles / O-3=100 / 100 / 0.3 (mass ratio).
[0212] (Preparation of protective layer-forming coating solution S9) A protective layer-forming coating solution S9 was prepared in the same manner as the protective layer-forming coating solution S1, except that the polymerization initiator O-1 was changed to a polymerization initiator O-4 (manufactured by IGM Resins, product name Omnirad 369).
[0213] [O-4]
[0214] (Preparation of protective layer-forming coating solution S10) A protective layer-forming coating solution S10 was prepared in the same manner as the protective layer-forming coating solution S1, except that the polymerization initiator O-1 was changed to a polymerization initiator O-5 (manufactured by IGM Resins, product name Omnirad 379EG).
[0215] [O-5]
[0216] (Preparation of Coating Solution S11 for Forming Protective Layer) Coating Solution S11 for forming protective layer was prepared in the same manner as for Coating Solution S1 for forming protective layer, except that the polymerization initiator O-1 was changed to polymerization initiators O-6 (benzophenone, manufactured by Tokyo Chemical Industry Co., Ltd.) and O-7 (product name Omnirad TPO H, manufactured by IGM Resins) and the contents were changed to the following ratio: TMPT / titanium oxide particles / O-6 / O-7=100 / 100 / 1 / 2 (mass ratio)
[0217] [O-6]
[0218] [O-7]
[0219] (Preparation of protective layer-forming coating liquid S12) A protective layer-forming coating liquid S12 was prepared in the same manner as the protective layer-forming coating liquid S11, except that the curable compound M-1 was changed to a curable compound M-2 (product name M-DPH-6E, manufactured by Shin-Nakamura Chemical Co., Ltd.).
[0220] (Preparation of protective layer-forming coating solution S13) A protective layer-forming coating solution S13 was prepared in the same manner as the protective layer-forming coating solution S1, except that the polymerization initiator O-1 was changed to a polymerization initiator O-8 represented by the following structure.
[0221] [O-8]
[0222] (Preparation of protective layer-forming coating solution S14) A protective layer-forming coating solution S14 was prepared in the same manner as the protective layer-forming coating solution S1, except that the polymerization initiator O-1 was changed to a polymerization initiator O-9 represented by the following structure.
[0223] [O-9]
[0224] <Preparation of Single-Layer Photoreceptors> Single-layer photoreceptors (photoreceptors A1 to A14) were prepared by the following procedure.
[0225] [Example 1] An aluminum cylinder with a machined surface and a diameter of 30 mm and a length of 244 mm was dip-coated with coating solution P1 for forming an undercoat layer, to form an undercoat layer with a film thickness of 0.3 μm after drying. Coating solution Q1 for forming a single-layer photosensitive layer was dip-coated onto the undercoat layer and dried at 125°C for 24 minutes, to form a single-layer photosensitive layer with a film thickness of 30 μm after drying. Coating solution S1 for forming a protective layer was ring-coated onto the single-layer photosensitive layer and dried at room temperature for 1 minute. After that, 1.1 W / cm 365 nm LED light was applied to the single-layer photosensitive layer while rotating the photoreceptor at 60 rpm under a nitrogen atmosphere. 2 Irradiation for 2 minutes at an intensity of 132 J / cm 2 ) to provide a protective layer having a thickness of 2 μm after curing, thereby producing photoreceptor A1.
[0226] Example 2 Photoreceptor A2 was produced in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S2.
[0227] Example 3 Photoreceptor A3 was produced in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S3.
[0228] Example 4 Photoreceptor A4 was produced in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S4.
[0229] Example 5 Photoreceptor A5 was produced in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S5.
[0230] Example 6 Photoreceptor A6 was produced in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S6.
[0231] Example 7 Photoreceptor A7 was produced in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S7.
[0232] Example 8 Photoreceptor A8 was produced in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S8.
[0233] Comparative Example 1 Photoreceptor A9 was produced in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S9.
[0234] Comparative Example 2 Photoreceptor A10 was produced in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S10.
[0235] Comparative Example 3 Photoreceptor A11 was produced in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S11.
[0236] Comparative Example 4 Photoreceptor A12 was produced in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S12.
[0237] Comparative Example 5 Photoreceptor A13 was produced in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S13.
[0238] Comparative Example 6 Photoreceptor A14 was produced in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S14.
[0239] <Measurement of Martens Hardness and Elastic Deformation Rate> The photoreceptors A1 to A14 obtained in the examples and comparative examples were measured from the surface side of the photoreceptor using a microhardness tester (Fischer: FISCHERSCOPE HM2000) under the following measurement conditions in an environment of a temperature of 25°C and a relative humidity of 50%. The Martens hardness and elastic deformation rate of each sample are shown in Table 1.
[0240] (Conditions for measuring Martens hardness and elastic deformation rate) Indenter: Vickers square pyramidal diamond indenter with a facing angle of 136° Maximum indentation load: 0.2 mN Loading time: 10 seconds Unloading time: 10 seconds
[0241] The Martens hardness was calculated using the following formula: Martens hardness (N / mm 2 ) = Maximum indentation load / Indentation area at maximum indentation load
[0242] The elastic deformation rate is a value defined by the following formula, and is the ratio of the work performed by the membrane due to its elasticity when unloading to the total work required for pressing: Elastic deformation rate (%) = (We / Wt) x 100 In the above formula, the total work Wt (nJ) represents the area surrounded by A-B-D-A in Figure 2, and the elastic deformation work We (nJ) represents the area surrounded by C-B-D-C. The larger the elastic deformation rate, the less likely deformation in response to load will remain, and an elastic deformation rate of 100 means that no deformation will remain.
[0243] In the present invention, the Martens hardness is 170 N / mm 2 The cases where the elastic deformation rate was 25% or more were evaluated as "pass."
[0244] <Evaluation of Image Flow> The layered photoreceptors A1 to A14 obtained in the above Examples and Comparative Examples were mounted in an electrophotographic printer, and printing was performed in an environment of a temperature of 32°C and a relative humidity of 80%, and the image was observed at room temperature and room humidity. The degree of image flow was evaluated by rating it as ◯ (pass) when no image flow (image blur) was observed and × (fail) when image flow (image blur) was observed. The results are shown in Table 1.
[0245]
[0246] <Discussion> All of Examples 1 to 8 had high Martens hardness and elastic deformation rate. Furthermore, all of Examples 1 to 8 were able to achieve results in which image deletion was suppressed.
[0247] From the results of the above examples and comparative examples, as well as the results of tests conducted by the inventors up to now, it can be considered that if the protective layer has a structure represented by the following formula (1), the Martens hardness and elastic deformation rate will be high, and image deletion can be suppressed.
[0248] [Formula (1)]
[0249] In the compound (8) of Comparative Example 5, the number of carbon atoms in the substituent R1 in the above formula (1) is 1, so it is considered that the number of carbon atoms in the substituent R1 must be at least greater than this, and therefore the number of carbon atoms must be 2 or more, preferably 3 or more. From the viewpoint of curability, it is considered that R2 may be a single bond or a carbonyl group. 3 Any substituent can be used for each of the groups because they do not affect the steric hindrance around the oxime ester moiety, but they are preferably non-polar substituents from the viewpoint of preventing them from affecting particle dispersion. From this viewpoint, they may each independently be any of a hydrogen atom, a halogen atom, a nitro group, an acyl group which may have a substituent, an alkyl group having 1 to 20 carbon atoms which may have a substituent, and an aryl group which may have a substituent, and it is also considered that they may be bonded to each other to form a cyclic structure.
Claims
1. An electrophotographic photoreceptor having a photosensitive layer and a protective layer in this order on a conductive support, wherein the protective layer contains a polymer having a structure represented by the following formula (1): [Formula (1)] (In formula (1), R represents an organic group having two or more carbon atoms. R represents a single bond or a carbonyl group. X, Y, and R 3 each independently represents an arbitrary substituent; T represents a bond to an arbitrary atom.
2. The electrophotographic photoreceptor according to claim 1, wherein the protective layer contains a polymer having a structure represented by the following formula (2): [Formula (2)] (In formula (2), R1 represents an organic group having two or more carbon atoms. R2 represents a single bond or a carbonyl group. R3, R4, R5, R6, and R7 each independently represent a hydrogen atom, a halogen atom, a nitro group, an acyl group which may have a substituent, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group which may have a substituent, and may be bonded to each other to form a cyclic structure. Y each independently represent a hydrogen atom, a halogen atom, a nitro group, an acyl group which may have a substituent, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group which may have a substituent. T represents a bond to any atom.) 3. An electrophotographic photoreceptor having a photosensitive layer and a protective layer in this order on a conductive support, wherein the protective layer contains a polymer of a compound represented by the following formula (3): [Formula (3)] (In formula (3), R represents an organic group having two or more carbon atoms. R represents a single bond or a carbonyl group. X, Y, and R 3 and R8 each independently represent any substituent.
4. The electrophotographic photoreceptor according to claim 3, wherein the protective layer contains a polymer of a compound represented by the following formula (4): [Formula (4)] (In formula (4), R1 represents an organic group having 2 or more carbon atoms. R2 represents a single bond or a carbonyl group. R3, R4, R5, R6, and R7 each independently represent a hydrogen atom, a halogen atom, a nitro group, an acyl group which may have a substituent, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group which may have a substituent, and may be bonded to each other to form a cyclic structure. Y each independently represent a hydrogen atom, a halogen atom, a nitro group, an acyl group which may have a substituent, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group which may have a substituent. R8 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group which may have a substituent.) 5. The electrophotographic photoreceptor according to claim 2 or 4, wherein at least one of R3, R4, R5, R6 and R7 is an acyl group which may have a substituent.
6. The electrophotographic photoreceptor according to claim 5, wherein the acyl group which may have a substituent has a structure represented by formula (5). [Formula (5)] (In formula (5), R9 represents a hydrogen atom, a halogen atom, a nitro group, an acyl group which may have a substituent, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group which may have a substituent. When there are two or more R9's, they may be bonded to each other to form a cyclic structure. U represents a bond to the nitrogen to which R3 is bonded, or a bond to the carbon to which any of R4, R5, R6, and R7 is bonded.) 7. The electrophotographic photoreceptor according to any one of claims 1 to 4, wherein the protective layer has a chain-polymerizable functional group.
8. The electrophotographic photoreceptor according to claim 7, wherein the chain polymerizable functional group is an acryloyloxy group or a methacryloyloxy group.
9. The electrophotographic photoreceptor according to claim 6, wherein said R6 has a structure represented by formula (5).
10. The above R 1The electrophotographic photoreceptor according to any one of claims 1 to 4, wherein the organic group is an acyl group which may have a substituent, an alkyl group which may have a substituent, or an aryl group which may have a substituent.
11. The electrophotographic photoreceptor according to any one of claims 1 to 4, wherein R1 is a structure selected from the group consisting of the following formulas (6) to (8): [Formula (6)] [Formula (7)] [Formula (8)] (In formulas (6), (7), and (8), W represents a bond to the carbon to which R is bonded.) 12. The above R 3 5. The electrophotographic photoreceptor according to claim 1, wherein: is an alkyl group having 1 to 20 carbon atoms which may have a substituent.
13. The electrophotographic photoreceptor according to any one of claims 1 to 4, wherein the protective layer contains metal oxide particles.
14. The electrophotographic photoreceptor according to claim 13, wherein said metal oxide particles are titanium oxide.
15. An electrophotographic photoreceptor as described in claim 13, characterized in that the protective layer contains the structure represented by formula (1) in a ratio of 0.03 mol % or more and 2 mol % or less relative to 100 mol % of the metal oxide particles in the protective layer.
16. The electrophotographic photoreceptor according to claim 1 or 3, wherein the photosensitive layer is a single-layer type photosensitive layer.
17. An electrophotographic photoreceptor cartridge comprising the electrophotographic photoreceptor according to claim 1 or 3.
18. An image forming apparatus comprising the electrophotographic photoreceptor according to claim 1 or 3.
Citation Information
Patent Citations
Photoconductive film and electrophotographic body formed by using said film
JP1989187569A
Single-layer electrophotographic photoreceptor and image forming apparatus
JP2009229948A
Electrophotographic photoreceptor, method for manufacturing the same, and electrophotographic image forming apparatus
JP2018013676A