Backing material, ultrasound probe, ultrasound diagnosis device, and curable resin composition

The use of thermally conductive particles blended with specific resin formulations in the backing material addresses the softness and processing issues of existing materials, enhancing heat dissipation and ultrasonic attenuation, and improving the performance and productivity of ultrasound probes.

WO2024204614A1PCT designated stage expired Publication Date: 2024-10-03FUJIFILM CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012827
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing backing materials for ultrasound probes face challenges with softness, leading to processing difficulties and inadequate strength, which affects their performance in providing both high heat dissipation and ultrasonic attenuation properties.

Method used

A backing material composed of thermally conductive particles blended with specific resin formulations, such as reaction-cured products of epoxy resins with polyurethane, polyether, or polyisocyanate structures, offering improved heat dissipation, ultrasonic attenuation, and processability, along with a curable resin composition suitable for forming these materials.

Benefits of technology

The solution provides a backing material with enhanced heat dissipation, ultrasonic attenuation, and workability, enabling efficient heat management and vibration absorption, thus improving the performance and productivity of ultrasound probes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012827_03102024_PF_FP_ABST
    Figure JP2024012827_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a backing material for ultrasound probes, the backing material comprising thermally conductive particles and a resin. In the backing material, the resin contains any one of components (A) to (C) wherein the component (A) is a reaction-cured product of an epoxy resin having a polyurethane structure and a polyamine compound, the component (B) is a reaction-cured product of an epoxy resin and a polyamine compound and has a polyether structure, and the component (C) is a reaction-cured product of a polyisocyanate compound and a polyamine compound. The resin has a loss tangent in a range of 0 to 50°C of 0.06 or more and a loss tangent in a range of -20 to 110°C of less than 1.50. The storage elastic modulus of the backing material in a range of 0 to 50°C is 1000 MPa or more. The content of the resin in the backing material is 25 to 50% by volume. Also provided are: an ultrasound probe; an ultrasound diagnosis device; and a curable resin composition.
Need to check novelty before this filing date? Find Prior Art

Description

Backing material, ultrasonic probe, ultrasonic diagnostic device and curable resin composition

[0001] The present invention relates to a backing material, an ultrasonic probe, an ultrasonic diagnostic device, and a curable resin composition.

[0002] An ultrasonic measurement device uses an ultrasonic probe that irradiates an object or region under test (hereinafter simply referred to as the object) with ultrasonic waves, receives the reflected waves (echoes), and outputs a signal. The reflected waves received by this ultrasonic probe are converted into electrical signals and displayed as an image. This allows the inside of the object to be visualized and observed.

[0003] During diagnosis, an ultrasound probe transmits an ultrasound signal from the front of the piezoelectric element into the subject by, for example, contacting the acoustic lens side of the ultrasound probe with the subject and driving the piezoelectric element. This ultrasound signal is focused at a desired location within the subject by electronic focusing based on the drive timing of the piezoelectric element and focusing by the acoustic lens. By controlling the drive timing of the piezoelectric element, the ultrasound signal can be transmitted to a desired area within the subject, and an ultrasound image (tomographic image) of the desired area can be obtained by receiving and processing echo signals from the subject. Driving the piezoelectric element also emits an ultrasound signal from the back side. For this reason, a backing material is placed on the back of the piezoelectric element to absorb (attenuate) the ultrasound signal to the back side, thereby avoiding the adverse effect of transmitting the normal ultrasound signal into the subject along with the ultrasound signal (reflected signal) from the back side. In addition to the high ultrasonic attenuation property described above, the backing material is required to have all the following properties: high heat dissipation property that can efficiently dissipate the heat emitted from the piezoelectric element when the ultrasonic probe is driven; and processability that can produce the backing material for the ultrasonic probe with high productivity while suppressing the occurrence of deformation, breakage, etc.

[0004] Previously, techniques have been known for imparting high heat dissipation properties to backing materials by adding a thermally conductive filler. For example, Patent Document 1 describes an acoustic backing composition containing an ethylene-vinyl acetate copolymer with a vinyl acetate content of 20 to 80% by weight and a thermally conductive filler. Furthermore, Patent Document 2 describes a backing material (backing material) for an ultrasonic probe, which contains a main material made of nitrile rubber, butyl rubber, or urethane rubber and a thermally conductive filler made of aluminum nitride, silicon carbide, copper, boron nitride, or graphite.

[0005] JP 2006-033801 A JP 2000-165995 A

[0006] The inventors have conducted research and found that while the acoustic backing composition described in Patent Document 1 provides an acoustic backing material that combines high heat dissipation and high ultrasonic attenuation, the softness of the ethylene-vinyl acetate copolymer results in insufficient strength, making processing difficult and problematic for use as a backing material. Furthermore, the backing load material (backing material) described in Patent Document 2 also combines high heat dissipation and high ultrasonic attenuation, but is difficult to process due to the softness and processability of the rubber material, making it also problematic for use as a backing material. The present invention aims to provide a backing material that combines excellent ultrasonic attenuation and excellent processability in a backing material that has enhanced heat dissipation properties due to the incorporation of thermally conductive particles, as well as an ultrasonic probe and an ultrasonic diagnostic device that include this backing material. Another objective of the present invention is to provide a curable resin composition suitable for forming the backing material.

[0007] The above-mentioned problems of the present invention have been solved by the following means. [1] A backing material for an ultrasonic probe, comprising thermally conductive particles and a resin, wherein the resin comprises any one of the following (A) to (C): (A) a reaction-cured product of an epoxy resin having a polyurethane structure and a polyamine compound, (B) a reaction-cured product of an epoxy resin and a polyamine compound, the reaction-cured product having a polyether structure, or (C) a reaction-cured product of a polyisocyanate compound and a polyamine compound; wherein the resin has a loss tangent of 0.06 or more in the range of 0 to 50°C and a loss tangent of less than 1.50 in the range of -20 to 110°C, the backing material has a storage modulus of 1000 MPa or more in the range of 0 to 50°C, and the content of the resin in the backing material is 25 to 50% by volume. [2] The backing material according to [1], wherein the thermally conductive particles comprise at least one of metal particles and ceramic particles. [3] An ultrasonic probe comprising the backing material according to [1] or [2]. [4] An ultrasonic diagnostic device using the ultrasonic probe described in [3]. [5] A curable resin composition for forming the backing material described in [1] or [2], wherein the curable resin composition comprises the thermally conductive particles and any one of the following (a) to (c) as a resin component: (a) a combination of an epoxy resin having a polyurethane structure and a polyamine compound, (b) a combination of an epoxy resin and a polyamine compound, wherein at least one of the epoxy resin and the polyamine compound has a polyether structure, (c) a combination of a polyisocyanate compound and a polyamine compound; and the viscosity of the curable resin composition is 5000 Pa sec or less at 25°C and a shear rate of 0.01 / sec.

[0008] In the present invention, a numerical range expressed using "to" means a range that includes the numerical values ​​written before and after "to" as the lower and upper limits.

[0009] The backing material of the present invention is a backing material that has heat dissipation properties due to the incorporation of thermally conductive particles, and has excellent ultrasonic attenuation and processability. Furthermore, the ultrasonic probe and ultrasonic diagnostic device of the present invention include the backing material having the above properties. Furthermore, the curable resin composition of the present invention is suitable for forming the backing material.

[0010] FIG. 1 is a perspective view of an example of a convex ultrasonic probe, which is one aspect of an ultrasonic probe.

[0011] [Backing Material] The backing material of the present invention is a backing material for an ultrasonic probe, comprising thermally conductive particles and a resin, wherein the resin comprises any one of the following (A) to (C): (A) a reaction-cured product of an epoxy resin having a polyurethane structure and a polyamine compound, (B) a reaction-cured product of an epoxy resin and a polyamine compound, the reaction-cured product having a polyether structure, or (C) a reaction-cured product of a polyisocyanate compound and a polyamine compound; the resin has a loss tangent of 0.06 or more in the range of 0 to 50°C and a loss tangent of less than 1.50 in the range of -20 to 110°C, the backing material has a storage modulus of 1000 MPa or more in the range of 0 to 50°C, and the content of the resin in the backing material is 25 to 50% by volume. The details of why the backing material of the present invention has excellent ultrasonic attenuation and processability are not clear, but are thought to be as follows.

[0012] The backing material of the present invention is a backing material for an ultrasonic probe that contains thermally conductive particles and a resin with specific viscoelastic properties. By using the backing material, the thermally conductive particles provide high heat dissipation while exhibiting excellent ultrasonic attenuation and excellent processability. Specifically, the resin has a loss tangent of 0.06 or greater in the temperature range of 0 to 50°C, which allows it to exhibit excellent ultrasonic attenuation. It is believed that when ultrasonic waves are irradiated onto a resin with this property, the polymer molecular chains that make up the resin absorb the vibration energy and consume it as their own kinetic energy, thereby dissipating the ultrasonic waves. Furthermore, the resin has a loss tangent of less than 1.50 in the temperature range of -20 to 110°C, which makes it less likely to soften even when the resin temperature increases during processing such as dicing. Furthermore, the backing material has a storage modulus of 1000 MPa or greater in the temperature range of 0 to 50°C, which makes it less likely to slip due to stress during processing, thereby allowing it to exhibit excellent processability. The present inventors have also discovered that a resin having the above-mentioned specific viscoelastic properties can be realized by using a specific amount of a resin selected from (A) a reaction-cured product of an epoxy resin having a polyurethane structure and a polyamine compound, (B) a reaction-cured product of an epoxy resin and a polyamine compound, the reaction-cured product having a polyether structure, and (C) a reaction-cured product of a polyisocyanate compound and a polyamine compound. The reason why a resin containing any of these (A) to (C) has the above-mentioned specific viscoelastic properties is not clear, but it is thought that this is related to the fact that the reaction-cured products of these (A) to (C) have many polar functional groups (urethane bonds, ether bonds, urea bonds) in the molecular chain and have strong intermolecular interactions.

[0013] The backing material of the present invention will be described in detail below.

[0014] (Loss Tangent of Resin) The loss tangent of the resin contained in the backing material of the present invention is 0.06 or more in the range of 0 to 50°C, and less than 1.50 in the range of -20 to 110°C. A loss tangent of 0.06 or more in the range of 0 to 50°C means that the minimum value of the loss tangent in the range of 0 to 50°C is 0.06 or more. The minimum value of the loss tangent in the range of 0 to 50°C is not particularly limited as long as it is 0.06 or more, and is usually 0.40 or less. The minimum value of the loss tangent in the range of 0 to 50°C may be in the range of 0.06 to 0.40, preferably 0.06 to 0.30, more preferably 0.06 to 0.20, even more preferably 0.06 to 0.15, and particularly preferably 0.06 to 0.12. A loss tangent of less than 1.50 in the range of -20 to 110°C means that the maximum value of the loss tangent in the range of -20 to 110°C is less than 1.50. The maximum value of the loss tangent in the range of -20 to 110°C is not particularly limited as long as it is less than 1.50, and is typically 0.10 or greater. The maximum value of the loss tangent in the range of -20 to 110°C may be 0.10 to 1.50, preferably 0.10 to 1.25, more preferably 0.10 to 1.00, even more preferably 0.10 to 0.75, and particularly preferably 0.10 to 0.55. The loss tangent of the resin is measured by the method described in the Examples below. The above "loss tangent in the range of 0 to 50°C" and "loss tangent in the range of -20 to 110°C" are values ​​rounded to two decimal places.

[0015] (Storage Modulus of Backing Material) The storage modulus of the backing material of the present invention in the range of 0 to 50°C is 1000 MPa or more. A storage modulus of 1000 MPa or more in the range of 0 to 50°C means that the minimum value of the storage modulus in the range of 0 to 50°C is 1000 MPa or more. The minimum value of the storage modulus in the range of 0 to 50°C is preferably 2000 MPa or more, more preferably 2500 MPa or more, even more preferably 3000 MPa or more, and particularly preferably 3300 MPa or more. The minimum value of the storage modulus in the range of 0 to 50°C is usually less than 8000 MPa. That is, the minimum value of the storage modulus in the range of 0 to 50°C may be in the range of 1000 MPa or more and less than 8000 MPa, preferably 2000 MPa or more and less than 8000 MPa, more preferably 2500 MPa or more and less than 8000 MPa, still more preferably 3000 MPa or more and less than 8000 MPa, and particularly preferably 3300 MPa or more and less than 8000 MPa. The storage modulus of the backing material is measured by the method described in the examples below.

[0016] (Attenuation Rate of Backing Material) The attenuation rate of the backing material of the present invention is preferably more than 0.8 dB / (mm MHz), more preferably more than 2.5 dB / (mm MHz), even more preferably more than 3.0 dB / (mm MHz), particularly preferably more than 3.5 dB / (mm MHz), and most preferably more than 4.0 dB / (mm MHz). The attenuation rate of the backing material is measured by the method described in the Examples below.

[0017] <Resin> The resin contained in the backing material of the present invention includes any one of the following (A) to (C): (A) a reaction-cured product of an epoxy resin having a polyurethane structure and a polyamine compound; (B) a reaction-cured product of an epoxy resin and a polyamine compound, the reaction-cured product having a polyether structure; (C) a reaction-cured product of a polyisocyanate compound and a polyamine compound. When a reaction-cured product of an epoxy resin having a polyurethane structure and a polyamine compound contains a polyether structure, it is classified as (A) above, not (B) above. Therefore, the epoxy resin in the reaction-cured product of (B) above does not have a polyurethane structure. When a reaction-cured product of a polyisocyanate compound and a polyamine compound contains a polyether structure, it is also classified as (C) above. From the viewpoint of further improving processability, the resin contained in the backing material of the present invention preferably contains (C) above.

[0018] [(A) Reaction Cured Product of Epoxy Resin Having a Polyurethane Structure and Polyamine Compound] (Epoxy Resin Having a Polyurethane Structure) The epoxy resin having a polyurethane structure can be used without any particular limitation as long as it is an epoxy resin having a polyurethane structure and an epoxy group. The number of epoxy groups in the epoxy resin having a polyurethane structure is usually 2 or more, preferably 2 to 4, and more preferably 2 to 3. Commercially available epoxy resins having a polyurethane structure are generally, for example, epoxy resins having a polyurethane structure with a number average molecular weight of 200 to 20,000, and specific examples thereof include the following: ADEKA RESIN EPU-6, ADEKA RESIN EPU-7N, ADEKA RESIN EPU-11F, ADEKA RESIN EPU-15F, ADEKA RESIN EPU-1395, ADEKA RESIN EPU-73B, ADEKA RESIN EPU-17, ADEKA RESIN EPU-17T-6, ADEKA RESIN EPU-1001 (all trade names, manufactured by ADEKA Corporation), EPOKY 802-30CX, EPOKY 803, EPOKY 820-40CX, EPOKY 830, EPOKY 834, EPOKY 840, EPOKY 815, EPOKY 837, EPOKY 810ST, EPOKY 505-15 (all trade names, manufactured by Mitsui Chemicals, Inc.), and the like. Among these, ADEKA RESIN EPU-7N, ADEKA RESIN EPU-11F, and EPU-17 (all trade names, manufactured by ADEKA Corporation) are preferred because they have excellent mixability with thermally conductive particles.

[0019] The epoxy group equivalent of the epoxy resin having a polyurethane structure is not particularly limited, and is preferably 170 to 2,000 g / mol, and more preferably 200 to 500 g / mol. The epoxy group equivalent refers to the mass (g) of the epoxy resin having a polyurethane structure per 1 mol of epoxy groups. The viscosity of the epoxy resin having a polyurethane structure at 25°C is not particularly limited, and is preferably 200 to 200,000 mPa·s, and more preferably 600 to 30,000 mPa·s. The viscosity is a value measured by the method described in the Examples below. The same applies to the viscosity described in (A) to (C) below.

[0020] (Polyamine Compound) The polyamine compound to be reacted with the epoxy resin having a polyurethane structure can be any polyamine compound having two or more amino groups, and is preferably a polyamine compound typically used as a curing agent for epoxy resins. The polyamine compound may be any of aliphatic polyamine compounds (chain aliphatic polyamine compounds in which amino groups are bonded to an aliphatic chain (however, chain aliphatic polyamine compounds do not have a ring structure), cycloaliphatic polyamine compounds in which amino groups are bonded to an aliphatic ring directly or via an aliphatic chain (however, cycloaliphatic polyamine compounds may have nitrogen atoms constituting amino groups as ring-constituting atoms of the aliphatic ring), and aliphatic polyamine compounds having an aromatic ring (aliphatic polyamine compounds in which amino groups are bonded to an aliphatic chain or aliphatic ring and also have an aromatic ring)), or a mixture thereof. Aliphatic polyamine compounds are preferred due to their excellent reactivity. As mentioned above, the polyamine compound may have a ring structure. In addition to the nitrogen atom, the polyamine compound may contain heteroatoms such as oxygen atoms and sulfur atoms, and may have a polyether structure. Preferred examples of the polyether structure include polyether structures having a number average molecular weight of 200 to 6000. The number of amino groups in the polyamine compound is preferably two or three. The two or more amino groups in the polyamine compound may be amino groups having active hydrogen, and specifically, unsubstituted amino groups (-NH 2 ) and a mono-substituted amino group having one active hydrogen atom, and 2). The monosubstituted amino group having one active hydrogen may be incorporated into the compound in the form of >NH. The polyamine compound may have a disubstituted amino group (amino group without active hydrogen) in addition to the two or more amino groups (amino groups having active hydrogen) that the polyamine compound has. The number of active hydrogens derived from the amino groups that the polyamine compound has may be two or more, preferably 3 to 6, and more preferably 4 to 6. Among these, the polyamine compound preferably has an unsubstituted amino group (-NH 2 ), and preferably has two or more unsubstituted amino groups (—NH 2 It is more preferable that the polyamine compound has two or three of the above-mentioned groups. The polyamine compound may be a low molecular weight compound or a high molecular weight compound.

[0021] Specific examples of polyamine compounds include the following: For example, chain aliphatic polyamine compounds include diethylenetriamine, triethylenetetramine, tetraethylenepentamine, dipropylenediamine, diethylaminopropylamine, hexamethylenediamine, and 2,2,4-trimethylhexamethylenediamine. Furthermore, chain aliphatic polyamine compounds containing oxygen atoms include chain aliphatic polyamine compounds having a polyalkylene oxide structure such as a polyethylene oxide structure or a polypropylene oxide structure, such as JEFFAMINE D-230, JEFFAMINE D-400, JEFFAMINE D-2000, JEFFAMINE T-403, and JEFFAMINE T-5000 (all trade names, manufactured by HUNTSMAN). Examples of cyclic aliphatic polyamine compounds include N-aminoethylpiperazine, 4,4'-methylenebis(2-methylcyclohexane-1-amine), menthenediamine, isophoronediamine, bis(4-aminocyclohexyl)methane, and 1,3-bisaminomethylcyclohexane. Examples of aliphatic polyamine compounds having an aromatic ring (polyamine compounds having an amino group bonded to an aliphatic chain or aliphatic ring and also having an aromatic ring) include m-xylylenediamine, Gascamine 240, and Gascamine 328 (all trade names, manufactured by Mitsubishi Gas Chemical Company, Inc.). Examples of aromatic polyamine compounds include m-phenylenediamine, diaminodiphenylmethane, and diaminodiphenylsulfone. Other examples include Elastomer 250P, Elastomer 650P, Elastomer 1000P, and Porea SL-100A (all trade names, manufactured by Kumiai Chemical Co., Ltd.). Among these polyamine compounds, it is preferable to contain an aliphatic polyamine compound having an aromatic ring, because it has good reactivity and excellent intermolecular interaction. In particular, it is preferable to contain an aliphatic polyamine compound having an aromatic ring and a chain aliphatic polyamine compound not having an aromatic ring, from the viewpoint of further improving ultrasonic attenuation and processability in an embodiment containing the reaction cured product of (A).

[0022] The amino group equivalent of the polyamine compound is not particularly limited, and is, for example, preferably 30 to 12,000 g / mol, more preferably 30 to 3,000 g / mol, and even more preferably 30 to 1,200 g / mol. The amino group equivalent refers to the mass (g) of the polyamine compound per 1 mol of amino groups. The polyamine compound may be solid or liquid at 25°C. When the polyamine compound is liquid at 25°C, the viscosity of the polyamine compound at 25°C is not particularly limited, and is, for example, preferably 1 to 30,000 mPa·s, more preferably 3 to 30,000 mPa·s, and even more preferably 3 to 20,000 mPa·s.

[0023] [(B) Reaction-cured product of an epoxy resin and a polyamine compound, which has a polyether structure] The reaction-cured product of (B) is a reaction-cured product of an epoxy resin and a polyamine compound having two or more amino groups, and can be used without any particular limitation as long as it has a polyether structure. The reaction-cured product of (B) can be obtained by either a reaction between an epoxy resin having a polyether structure and a polyamine compound not having a polyether structure, a reaction between an epoxy resin not having a polyether structure and a polyamine compound having a polyether structure, or a reaction between an epoxy resin having a polyether structure and a polyamine compound having a polyether structure, and the polyether structure possessed by the reaction-cured product obtained in this manner is usually a polyether structure with a number-average molecular weight of 200 to 6,000. Among these, the reaction cured product of (B) is preferably a reaction cured product of an epoxy resin having a polyether structure and a polyamine compound having no polyether structure, or a reaction cured product of an epoxy resin having no polyether structure and a polyamine compound having a polyether structure, and more preferably a reaction cured product of an epoxy resin having no polyether structure and a polyamine compound having a polyether structure, from the viewpoint of exhibiting a more preferable viscosity as a curable resin composition described later.

[0024] (Epoxy Resin) The number of epoxy groups in an epoxy resin is usually 2 or more, preferably 2 to 4, and more preferably 2 to 3. Commercially available epoxy resins having a polyether structure are generally, for example, epoxy resins having a polyether structure with a number average molecular weight of 200 to 6000, and specific examples include the following: Denacol EX-851, Denacol EX-832, Denacol EX-101, Denacol EX-103 (all trade names, manufactured by Nagase ChemteX Corporation), DER 732 (trade name, manufactured by Dow Chemical Company), Adeka Resin EP-4000 (trade name, manufactured by ADEKA Corporation), etc. In terms of excellent mechanical strength, those having a bisphenol structure are preferred, and Adeka Resin EP-4000, Denacol EX-103, etc. are preferred. Examples of epoxy resins that do not have a polyether structure include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol E type epoxy resins, novolac type epoxy resins, etc. From the viewpoint of excellent mechanical strength of the resulting reaction-cured product, bisphenol A type epoxy resins are preferred.

[0025] The epoxy group equivalent of the epoxy resin is not particularly limited, and is, for example, preferably 160 to 550 g / mol, more preferably 160 to 400 g / mol, and even more preferably 165 to 230 g / mol. The epoxy group equivalent refers to the mass (g) of the epoxy resin per 1 mol of epoxy groups. The viscosity of the epoxy resin at 25°C is not particularly limited, and is, for example, preferably 700 to 20,000 mPa·s, more preferably 1,000 to 20,000 mPa·s, and even more preferably 1,000 to 15,000 mPa·s.

[0026] (Polyamine Compound) Examples of polyamine compounds for obtaining the reaction cured product (B) include polyamine compounds that are reacted with the epoxy resin having a polyurethane structure in (A) described above, and the preferred ranges are the same. Commercially available polyamine compounds having a polyether structure are generally, for example, polyamine compounds having a polyether structure with a number average molecular weight of 200 to 6000, and specific examples are as follows. Among the polyamine compounds that are reacted with the epoxy resin having a polyurethane structure in (A) described above, preferred examples include JEFFAMINE D-230, JEFFAMINE D-400, JEFFAMINE D-2000, JEFFAMINE T-403, and JEFFAMINE T-5000 (all trade names, manufactured by HUNTSMAN). It is also preferable to use a mixture of multiple types of these compounds in order to adjust the average molecular weight and the mechanical strength of the resulting reaction cured product. For example, suitable mechanical strength can be obtained by mixing JEFFAMINE D-400 and JEFFAMINE D-2000, or by mixing JEFFAMINE D-230 and JEFFAMINE T-5000, both of which are trade names manufactured by HUNTSMANN.

[0027] [(C) Reaction Cured Product of Polyisocyanate Compound and Polyamine Compound] (Polyisocyanate Compound) The polyisocyanate compound can be any polyisocyanate compound having two or more isocyanato groups. For example, various polyisocyanate compounds used in the production of polyurethane and polyurea can be preferably used. The polyisocyanate compound may be either an aliphatic isocyanate compound (a compound in which an isocyanato group is bonded to an aliphatic chain or an aliphatic ring) or an aromatic isocyanate compound (a compound in which an isocyanato group is bonded to an aromatic ring), or a mixture thereof. The polyisocyanate compound may have a ring structure. The number of isocyanato groups in the polyisocyanate compound is preferably two or three, and more preferably two. Examples of polyisocyanate compounds include diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI), toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), metaxylylene diisocyanate (XDI), norbornane diisocyanate (NBDI), and 1,4-bis(isocyanatomethyl)cyclohexane (1,4-H6XDI). Furthermore, in terms of low reactivity and long pot life when producing a reaction cured product, aliphatic polyisocyanate compounds are preferred, with hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), metaxylylene diisocyanate (XDI), norbornane diisocyanate (NBDI) or 1,4-bis(isocyanatomethyl)cyclohexane (1,4-H6XDI) being more preferred, and metaxylylene diisocyanate (XDI) or norbornane diisocyanate (NBDI) being even more preferred. Furthermore, from the viewpoint of further improving ultrasonic attenuation, it is preferable to contain an aliphatic polyisocyanate compound having an aromatic ring and an aromatic polyisocyanate compound.

[0028] The isocyanato group equivalent of the polyisocyanate compound is not particularly limited and is, for example, preferably 50 to 500 g / mol, more preferably 50 to 250 g / mol. The isocyanato group equivalent means the mass (g) of the polyisocyanate compound per 1 mol of isocyanato groups. The polyisocyanate compound may be solid or liquid at 25°C. When the polyisocyanate compound is liquid at 25°C, the viscosity of the polyisocyanate compound at 25°C is not particularly limited and is, for example, preferably 1 to 30,000 mPa·s, more preferably 3 to 30,000 mPa·s, and even more preferably 3 to 20,000 mPa·s.

[0029] (Polyamine Compound) Examples of the polyamine compound for obtaining the reaction cured product (C) include the polyamine compounds that are reacted with the epoxy resin having a polyurethane structure in (A) described above, and unless otherwise specified, preferred ranges can also be adopted. As the polyamine compound, among the polyamine compounds that are reacted with the epoxy resin having a polyurethane structure in (A) described above, aromatic polyamine compounds having a polyether structure such as Elastomer 250P, Elastomer 650P, Elastomer 1000P, and Porea SL-100A (all trade names, manufactured by Kumiai Chemical Co., Ltd.) are preferred because of their low reactivity and long pot life when producing a reaction cured product.

[0030] The content of the reaction-cured product of any one of (A) to (C) above in the resin contained in the backing material of the present invention is not particularly limited as long as the effects of the present invention are achieved, and can be, for example, 15% by volume or more, preferably 20% by volume or more, more preferably 30% by volume or more, even more preferably 50% by volume or more, and particularly preferably 70% by volume or more. It is also preferable that all of the resin contained in the backing material of the present invention is composed of any one of (A) to (C) above.

[0031] The content of the resin in the backing material is 25 to 50% by volume, and preferably 30 to 50% by volume.

[0032] <Thermal Conductive Particles> As the thermal conductive particles, either inorganic or organic particles may be used as long as they have thermal conductivity (preferably a thermal conductivity of 30 W / m·K or more), and any thermal conductive particles that impart heat dissipation properties to the backing material may be used without any particular limitation. The shape of the particles is not particularly limited, and various shapes such as amorphous, spherical, fibrous, branched fibrous, and tabular shapes may be used. A spherical shape is preferred because it can increase the packing density. On the other hand, an anisotropic shape such as a fibrous or tabular shape is preferred because it can increase particle contact and improve heat dissipation. Furthermore, irregular particles are preferred because they can randomly reflect ultrasonic waves, thereby improving the ultrasonic attenuation of the backing material.

[0033] Examples of inorganic particles include metal particles made of metals such as silver, copper, gold, aluminum, iron, brass, tungsten, molybdenum, and zinc. Among these, tungsten or molybdenum particles are preferred due to their low electrical conductivity. Oxides, carbides, or nitrides of the above metal particles are also preferred, with aluminum trioxide (alumina, sapphire), zinc oxide, aluminum nitride, tungsten carbide, or molybdenum carbide being preferred. Inorganic particles such as silicon carbide and boron nitride are also preferred. That is, metal particles, ceramic particles, and the like are preferred as inorganic particles. Examples of organic particles include graphite, carbon nanotubes, and diamond. Of these, diamond is preferred due to its low electrical conductivity. The thermal conductivity of the thermally conductive particles is preferably 30 W / m·K or higher. The surfaces of the metal particles may be surface-treated. Examples of surface treatments include UV (ultraviolet) surface treatment, plasma surface treatment, corona surface treatment, silane coupling treatment, titanium coupling treatment, aluminum coupling treatment, and phosphate treatment. The surface treatment can change the functional groups on the particle surface, improve particle dispersibility in the resin, and improve thermal conductivity and ultrasonic attenuation by changing the interparticle distance. The thermally conductive particles preferably contain at least one of metal particles and ceramic particles.

[0034] The particle size of the thermally conductive particles is not particularly limited. From the viewpoint of maintaining high mechanical strength of the backing material (cured product) of the present invention while keeping the viscosity of the curable resin composition described below low, the particle size of the thermally conductive particles is, for example, preferably 1 to 300 μm, more preferably 5 to 100 μm, and even more preferably 8 to 30 μm. The "particle size" of the thermally conductive particles is the number average particle size, and is a value measured by the method described in the Examples described below.

[0035] The proportion of thermally conductive particles in the total amount of components other than the resin in the backing material is preferably 50% by volume or more, more preferably 60% by volume or more, and even more preferably 65% ​​by volume or more. It is also preferable that all components other than the resin in the backing material of the present invention are thermally conductive particles. The content of thermally conductive particles in the backing material is, for example, preferably 30 to 60% by volume, more preferably 30 to 55% by volume, and even more preferably 30 to 50% by volume. One type of thermally conductive particle may be used alone, or two or more types may be used in combination. In the present invention, the proportion and content of thermally conductive particles refer to the total amount when two or more types of thermally conductive particles are contained.

[0036] <Other Components> The backing material of the present invention may contain other components in addition to the above-mentioned resin and thermally conductive particles. It is preferable that the other components include hollow particles. By including hollow particles, ultrasonic attenuation can be further improved. As the hollow particles, any hollow particles commonly used to exhibit the effect of improving acoustic wave attenuation or ultrasonic attenuation can be used without any particular limitation. Either hollow glass particles or hollow resin particles may be used, with hollow resin particles being preferred. Preferred examples of hollow particles include glass balloons, hollow silica, senolite, phenolic resin microballoons, urea resin microballoons, plastic microballoons such as polymethyl methacrylate balloons, and thermally expandable microcapsules. Furthermore, as hollow particles, plastic microballoons whose surfaces are coated with an inert inorganic powder such as calcium carbonate may be used. Examples include the Matsumoto Microsphere series MFL-81GCA, MFL-SEVEN, MFL-HD30CA, MFL-HD60CA, and MFL-100MCA (all trade names, manufactured by Matsumoto Yushi Pharmaceutical Co., Ltd.). One type of hollow particle may be used alone, or two or more types may be used in combination. In the present invention, the content of hollow particles refers to the total amount when two or more types of hollow particles are contained. The particle size of the hollow particles is not particularly limited. From the viewpoint of maintaining a high mechanical strength of the backing material (cured product) of the present invention while keeping the viscosity of the curable resin composition described below low, the particle size of the hollow particles is, for example, preferably 1 to 300 μm, more preferably 5 to 100 μm, and even more preferably 20 to 80 μm. The "particle size" of the hollow particles is synonymous with the "particle size" of the thermally conductive particles described above. That is, the "particle size" of the hollow particles is a number average particle size, and is a value measured by the method described in the Examples below.

[0037] Other components may be included, such as dispersants, diluents, colorants, viscosity modifiers, plasticizers, and curing accelerators. The content of other components in the backing material may be, for example, 10 to 20% by volume.

[0038] A preferred embodiment of the backing material of the present invention is, for example, a backing material for an ultrasonic probe, which comprises a resin containing any one of (A) to (C) above and thermally conductive particles, wherein the resin has the specific viscoelastic properties and the backing material has a specific storage modulus, and which contains the hollow particles. In this embodiment, the contents of the respective components in the backing material are such that the resin content is 25 to 50% by volume, preferably 30 to 50% by volume, the thermally conductive particle content is preferably 30 to 60% by volume, more preferably 30 to 55% by volume, and even more preferably 30 to 50% by volume, and the hollow particle content is preferably 10 to 20% by volume.

[0039] <Curable Resin Composition> The backing material of the present invention is preferably formed using the curable resin composition of the present invention. The curable resin composition of the present invention is a curable resin composition for forming the backing material of the present invention, and the curable resin composition comprises thermally conductive particles and any one of the following (a) to (c) as a resin component: (a) a combination of an epoxy resin having a polyurethane structure and a polyamine compound, (b) a combination of an epoxy resin and a polyamine compound, wherein at least one of the epoxy resin and the polyamine compound has a polyether structure, or (c) a combination of a polyisocyanate compound and a polyamine compound; and the viscosity of the curable resin composition is 5000 Pa·s or less at 25°C and a shear rate of 0.01 / s.

[0040] The resin components in the curable resin composition of the present invention and the above (a) to (c) correspond to the resins and (A) to (C) in the backing material of the present invention when they are formed. Therefore, the epoxy resin and polyamine compound having a polyurethane structure in (a) can be described in the above (A) for the epoxy resin and polyamine compound having a polyurethane structure. The epoxy resin and polyamine compound in (b) can be described in the above (B) for the epoxy resin and polyamine compound. The polyisocyanate compound and polyamine compound in (c) can be described in the above (C) for the polyisocyanate compound and polyamine compound. In addition, when at least one of the epoxy resin and polyamine compound having a polyurethane structure contains a polyether structure in a combination of an epoxy resin and a polyamine compound having a polyurethane structure, it is classified as (a) rather than (b). Therefore, the epoxy resin in (b) does not have a polyurethane structure. Furthermore, in a combination of a polyisocyanate compound and a polyamine compound, if at least one of the polyisocyanate compound and the polyamine compound contains a polyether structure, it is classified as (c) above, not as (b) above. The blending ratio of the epoxy resin having a polyurethane structure and the polyamine compound in (a) above can be appropriately adjusted so that the resulting backing material of the present invention exhibits specific viscoelastic properties as a resin containing the above-mentioned (A) and exhibits a specific storage modulus as a backing material. The same applies to (b) and (c) above. That is, the blending ratio of the epoxy resin and the polyamine compound (provided that at least one of the epoxy resin and the polyamine compound has a polyether structure) in (b) above can be appropriately adjusted so that the resulting backing material of the present invention exhibits specific viscoelastic properties as a resin containing the above-mentioned (B) and exhibits a specific storage modulus as a backing material.The compounding ratio of the polyisocyanate compound and the polyamine compound in (c) above can be appropriately adjusted so that the resulting backing material of the present invention exhibits specific viscoelastic properties as a resin containing the above-mentioned (C) and exhibits a specific storage modulus as a backing material.

[0041] The thermally conductive particles in the curable resin composition of the present invention correspond to the thermally conductive particles in the backing material of the present invention. Therefore, the description of the thermally conductive particles in the backing material of the present invention can be applied to the thermally conductive particles in the curable resin composition of the present invention. In addition, the curable resin composition of the present invention can also contain other components described in the backing material of the present invention.

[0042] (Viscosity of Curable Resin Composition) The viscosity of the curable resin composition of the present invention is 5000 Pa·s or less at 25°C and a shear rate of 0.01 / s. The viscosity of the curable resin composition of the present invention is measured by the method described in the Examples below. When the curable resin composition of the present invention satisfies the above-mentioned specific viscosity, it has sufficient fluidity to be poured into a mold and can be molded into a desired shape. The viscosity of the curable resin composition of the present invention at 25°C and a shear rate of 0.01 / s is preferably 3000 Pa·s or less, more preferably 2000 Pa·s or less, even more preferably 1000 Pa·s or less, and particularly preferably 800 Pa·s or less.

[0043] The contents of the thermally conductive particles and resin components in the curable resin composition of the present invention are not particularly limited as long as the backing material of the present invention can be obtained. The content of any of the above (a) to (c) in the resin components of the curable resin composition of the present invention is not particularly limited as long as the effects of the present invention are achieved. For example, it may be 15% by volume or more, preferably 20% by volume or more, more preferably 30% by volume or more, even more preferably 50% by volume or more, and particularly preferably 70% by volume or more. There is no particular upper limit and it can be 100% by volume or less. The content of the resin components in the curable resin composition of the present invention is preferably 25 to 50% by volume, more preferably 30 to 50% by volume. The proportion of the thermally conductive particles in the total amount of components other than the above-mentioned resin components in the curable resin composition of the present invention is preferably 50% by volume or more, more preferably 60% by volume or more, and even more preferably 70% by volume or more. It is also preferable that all components other than the above-mentioned resin components in the curable resin composition of the present invention are thermally conductive particles. The content of the thermally conductive particles in the curable resin composition of the present invention is, for example, preferably 30 to 60% by volume, more preferably 30 to 55% by volume, and even more preferably 30 to 50% by volume. Furthermore, when the curable resin composition of the present invention contains the other components described above, the content of the other components in the curable resin composition of the present invention can be, for example, 10 to 20% by volume.

[0044] A preferred embodiment of the curable resin composition of the present invention includes, for example, a curable resin composition having the specific viscoelastic properties described above, and a resin component containing any one of (a) to (c) and thermally conductive particles, and the curable resin composition contains the hollow particles. In this embodiment, the contents of the respective components in the curable resin composition are as follows: the resin component content is preferably 25 to 50 volume %, more preferably 30 to 50 volume %, the thermally conductive particle content is preferably 30 to 60 volume %, more preferably 30 to 55 volume %, and even more preferably 30 to 50 volume %, and the hollow particle content is preferably 10 to 20 volume %.

[0045] <Method for Producing Backing Material> The curable resin composition of the present invention can be prepared by a conventional method. For example, the curable resin composition of the present invention can be obtained by kneading the components constituting the curable resin composition, including the thermally conductive particles described above, a resin component containing any one of the above (a) to (c), and other appropriate components, using a kneading device such as a rotation-revolution device such as a rotation-revolution mixer, a kneader, a pressure kneader, a Banbury mixer (continuous kneader), or a two-roll mill. The order in which the components are mixed is not particularly limited. The kneading conditions are not particularly limited, as long as the thermally conductive particles and other components that may be contained as appropriate are dispersed in the resin component.

[0046] The backing material of the present invention can be obtained by curing the curable resin composition of the present invention obtained in this manner. The curing conditions can be adjusted depending on the chemical reaction of the resin components contained in the curable resin composition of the present invention. For example, the backing material can be obtained by heat curing at 20 to 200°C for 5 to 500 minutes. The shape of the backing material is not particularly limited. For example, the backing material may be formed into a shape suitable for the backing material using a mold during curing. Alternatively, a sheet-like backing material may be obtained and then cut by dicing or the like to obtain the desired backing material. Furthermore, because the backing material of the present invention has excellent processability, the desired backing material can be produced while suppressing deformation, breakage, and the like, even when dicing into the desired shape at a pitch on the order of μm.

[0047] The backing material of the present invention is useful for medical devices, and can be preferably used in, for example, acoustic wave probes and acoustic wave measuring devices, and more preferably in ultrasound probes and ultrasound diagnostic devices. Note that, in the present invention, the term "acoustic wave measuring device" is not limited to an ultrasound diagnostic device or a photoacoustic wave measuring device, but refers to a device that receives acoustic waves reflected by or generated by an object and displays them as an image or signal intensity. In particular, the backing material of the present invention can be preferably used as a backing material for ultrasound probes, a backing material for photoacoustic wave measuring devices or ultrasound endoscopes, and a backing material for ultrasound probes equipped with capacitive micromachined ultrasound transducers (cMUTs) as an ultrasound transducer array. Specifically, the backing material of the present invention is preferably applied to, for example, the ultrasonic diagnostic apparatus described in JP-A-2003-169802, and the acoustic wave measuring apparatus such as the photoacoustic wave measuring apparatus described in JP-A-2013-202050 and JP-A-2013-188465.

[0048] <<Acoustic Wave Probe>> The configuration of an acoustic wave probe using the backing material of the present invention will be described in more detail below based on the configuration of an ultrasonic probe in an ultrasonic diagnostic device shown in Fig. 1. Note that an ultrasonic probe is a probe that uses ultrasonic waves, in particular, as the acoustic wave in an acoustic wave probe. Therefore, the basic structure of an ultrasonic probe can be applied directly to an acoustic wave probe.

[0049] [Ultrasonic Probe] The configuration of the ultrasonic probe of the present invention will be described in more detail below based on the configuration of an ultrasonic probe in an ultrasonic diagnostic device shown in Figure 1. The ultrasonic probe 10 is a major component of an ultrasonic diagnostic device and has the functions of generating ultrasonic waves and transmitting and receiving ultrasonic beams. As shown in Figure 1, the ultrasonic probe 10 is configured such that, from the tip (the surface that contacts the living body being examined), an acoustic lens 1, an acoustic matching layer 2, a piezoelectric element layer 3, and a backing material 4 are provided in this order. In recent years, a laminated structure has been proposed in which the transmitting ultrasonic transducer (piezoelectric element) and the receiving ultrasonic transducer (piezoelectric element) are made of different materials in order to receive higher-order harmonics.

[0050] <Piezoelectric Element Layer> The piezoelectric element layer 3 is a part that generates ultrasonic waves. Electrodes are attached to both sides of the piezoelectric element. When a voltage is applied, the piezoelectric element vibrates by repeatedly expanding and contracting, thereby generating ultrasonic waves.

[0051] The materials that make up the piezoelectric element include quartz crystal and LiNbO 3 , LiTaO 3 and KNbO 3 single crystals such as ZnO and AlN, thin films such as Pb(Zr,Ti)O 3 Inorganic ceramic piezoelectric materials, which are obtained by polarization-treating sintered bodies such as those based on the PZT system, are widely used. Generally, piezoelectric ceramics such as PZT (lead zirconate titanate), which have good conversion efficiency, are used. Furthermore, piezoelectric elements that detect high-frequency received waves require sensitivity over a wider bandwidth. For this reason, organic piezoelectric materials using organic polymeric materials such as polyvinylidene fluoride (PVDF) are used as piezoelectric elements suitable for high frequencies and wide bandwidths. Furthermore, Japanese Patent Laid-Open Publication No. 2011-071842 and other publications describe cMUTs that utilize MEMS (Micro Electro Mechanical Systems) technology, exhibiting excellent short-pulse and wide-band characteristics, and enabling mass production with minimal characteristic variation, resulting in an array structure. Any of these piezoelectric element materials can be preferably used in the present invention.

[0052] <Backing Material> The backing material 4 is provided on the back surface of the piezoelectric element layer 3, and by suppressing excess vibrations, it shortens the pulse width of ultrasound and contributes to improving the distance resolution in ultrasound diagnostic images. In the ultrasonic probe of the present invention, the backing material 4 includes the backing material of the present invention. The backing material of the present invention has excellent ultrasonic attenuation and processability, and also exhibits high heat dissipation properties due to the thermally conductive particles. Therefore, by using the backing material of the present invention or the curable resin composition of the present invention, it is possible to suppress excess vibrations radiated from the piezoelectric element layer 3 to the back surface side when the ultrasonic probe is driven, and a backing material 4 that can efficiently dissipate heat released from the piezoelectric element layer 3 can be obtained with good productivity while suppressing the occurrence of deformation, breakage, etc.

[0053] <Acoustic Matching Layer> The acoustic matching layer 2 is provided to reduce the difference in acoustic impedance between the piezoelectric element layer 3 and the subject to be examined, and to efficiently transmit and receive ultrasonic waves.

[0054] <Acoustic Lens> The acoustic lens 1 is provided to utilize refraction to focus ultrasonic waves in the slice direction and improve resolution. It is also required to be in close contact with the living body being examined, and to match the ultrasonic waves to the acoustic impedance of the living body (1.4 to 1.7 Mrayl for the human body). In other words, the acoustic lens 1 is made of a material whose acoustic speed is sufficiently slower than that of the human body and whose acoustic impedance is close to that of human skin, thereby improving the ultrasonic transmission and reception sensitivity.

[0055] The operation of the ultrasonic probe 10 configured as described above will now be described. A voltage is applied to the electrodes provided on both sides of the piezoelectric element layer 3 to resonate the piezoelectric element layer 3, and an ultrasonic signal is transmitted to the subject through the acoustic lens 1. During reception, the piezoelectric element layer 3 is vibrated by a reflected signal (echo signal) from the subject, and this vibration is electrically converted into a signal to obtain an image.

[0056] - Ultrasonic probe equipped with a cMUT (capacitive micromachined ultrasonic transducer) - When a cMUT device described in JP 2006-157320 A, JP 2011-71842 A, or the like is used in an ultrasonic transducer array, the sensitivity is generally lower than that of a transducer using a general piezoelectric ceramic (PZT). Note that, because a cMUT device is fabricated using MEMS technology, it is more easily mass-produced than a piezoelectric ceramic probe, and low-cost ultrasonic probes can be provided to the market.

[0057] Photoacoustic wave measurement device using photoacoustic wave imaging Photoacoustic wave imaging (PAI), as described in JP 2013-158435 A and other publications, irradiates the inside of the human body with light (electromagnetic waves) and displays an image of ultrasound waves generated when the irradiated light causes adiabatic expansion of human tissue, or the signal intensity of the ultrasound waves.

[0058] - Ultrasonic endoscope - The ultrasonic endoscope described in JP 2008-311700 A and the like includes an insertion section inserted into the body and an operating section connected to the proximal end of the insertion section. An ultrasonic probe is provided at the tip of the insertion section. By using a backing material containing the backing material of the present invention as the backing material constituting the ultrasonic probe, excess vibrations applied to the ultrasonic endoscope are suppressed, thereby improving the acoustic characteristics of the ultrasonic endoscope.

[0059] The present invention will be described in more detail below through examples, but the present invention should not be construed as being limited thereto.

[0060] Example <1> Preparation of Backing Material Compositions Backing material compositions (curable resin compositions) having the compositions shown in Tables 1-1 and 1-2 (hereinafter collectively referred to as "Table 1") were prepared. Specifically, the resin raw materials, thermally conductive particles (WC-3 and SiC-1), and hollow particles (B-1) were weighed out in the content ratios shown in Table 1 and mixed using a centrifugal mixer (product name: Awatori Rentaro Vacuum Type ARV-310, manufactured by Thinky Corporation) to prepare backing material compositions Nos. 101 to 125 and c01 to c18.

[0061] <2> Preparation of Backing Material Sheets The backing material composition prepared above was poured into a square mold with a side length of 30 mm and the desired depth, and cured by heating at 80°C for 18 hours and then at 150°C for 1 hour to prepare square backing material sheets with a side length of 30 mm and the desired thickness, which were used for the following measurements and evaluations. Backing material sheet Nos. 101 to 125 are backing materials of the present invention, and backing material sheet Nos. c01 to c18 are comparative backing materials. The depth of the mold used and the thickness of the resulting sheets were 2 mm and 0.5 mm, respectively.

[0062] <3> Measurement and Evaluation The backing material composition and backing material sheet were subjected to the following measurements and evaluations. The results are shown in Table 1.

[0063] (1) Measurement of Storage Modulus A square backing material sheet with a thickness of 0.5 mm was cut into 5 mm wide strips to prepare test specimens. The storage modulus of the prepared test specimens was measured using a dynamic viscoelasticity measuring device, ITK DVA-225 (trade name, manufactured by IT Measurement & Control Co., Ltd.), under the following conditions: a grip distance of 20 mm, a heating rate of 2°C / min, a measurement temperature range of -150°C to 250°C, and a frequency of 5 Hz. The minimum value of the storage modulus (hereinafter also abbreviated as "elastic modulus") in the range of 0 to 50°C was determined and evaluated based on the following criteria. - Evaluation Criteria (Elastic Modulus) - S: The elastic modulus is 3300 MPa or more and less than 8000 MPa. A: The elastic modulus is 3000 MPa or more and less than 3300 MPa. B: The elastic modulus is 2500 MPa or more and less than 3000 MPa. C: The elastic modulus is 2000 MPa or more and less than 2500 MPa. D: The elastic modulus is 1000 MPa or more and less than 2000 MPa. E: The elastic modulus is less than 1000 MPa.

[0064] (2) Attenuation Rate Based on the method described in JIS (Japanese Industrial Standards) Z 2354 (2012) "Method for measuring ultrasonic attenuation coefficient of solids," the intensity of the reflected echo was measured using a sing-around sound velocity measuring device (manufactured by Ultrasonic Industries, product name "Ultrasonic Sound Velocity Measuring Device UVM-2 Type"). The measurement was performed using a 2 MHz measuring probe in water at 25°C, and a 2 mm thick backing material sheet was used as the measurement specimen. The attenuation rate was calculated from the difference in the intensity of the reflected echo with and without the measurement specimen and the thickness of the measurement specimen, and evaluated based on the following criteria: - Evaluation Criteria (Attenuation Rate) - S: The attenuation rate is greater than 4.0 dB / (mm MHz). A: The attenuation rate is greater than 3.5 dB / (mm MHz) and is equal to or less than 4.0 dB / (mm MHz). B: The attenuation rate is greater than 3.0 dB / (mm MHz) and is equal to or less than 3.5 dB / (mm MHz). C: The attenuation rate is greater than 2.5 dB / (mm.MHz) and less than 3.0 dB / (mm.MHz). D: The attenuation rate is greater than 0.8 dB / (mm.MHz) and less than 2.5 dB / (mm.MHz). E: The attenuation rate is less than 0.8 dB / (mm.MHz).

[0065] (3) Viscosity The viscosity of the backing material composition was measured using a HAAKE MARS 40 rheometer (trade name, manufactured by Thermo Fisher Scientific) under the following conditions: temperature: 25°C, shear rate: 0.01 / sec, sensor: C35 2° / Ti, measurement mode: oscillation mode, frequency: 0.03 Hz, and evaluated based on the following criteria. - Evaluation criteria (viscosity) - S: Viscosity is 800 Pa·s or less. A: Viscosity is greater than 800 Pa·s and less than 1000 Pa·s. B: Viscosity is greater than 1000 Pa·s and less than 2000 Pa·s. C: Viscosity is greater than 2000 Pa·s and less than 3000 Pa·s. D: Viscosity is greater than 3000 Pa·s and less than 5000 Pa·s. E: Viscosity exceeds 5000 Pa·sec.

[0066] (4) Processability Using an automatic dicing saw DAD321 (trade name, manufactured by DISCO Corporation) and a 0.03 mm thick diamond blade, a 0.5 mm thick backing material sheet was cross-diced to form grooves 30 μm wide and 200 μm deep, and 20 vertical and 20 horizontal squares (400 squares in total) with dimensions of 200 μm x 200 μm per square were formed. The squares formed by this cross dicing were observed under a microscope, and the number of damaged and / or fallen squares out of the 400 squares was counted, and the processability was evaluated based on the following criteria. - Evaluation Criteria (Processability) - S: No damaged and / or fallen squares were present. A: The number of damaged and / or fallen squares was 1 to 4. B: The number of damaged and / or fallen squares was 5 to 20. C: The number of damaged and / or fallen squares is 21 or more and 40 or less. D: The number of damaged and / or fallen squares is 41 or more and 80 or less. E: The number of damaged and / or fallen squares is 81 or more.

[0067]

[0068]

[0069] (Resin raw materials) R-1 to R-23 and PR-1 to PR-10: R-1 to R-23 and PR-1 to PR-10 listed in Tables A-1 to A-3 below (hereinafter collectively referred to as "Table A"), which are obtained by mixing the base resin and curing agent in the blending ratio listed in Table A. S-1, SE-1, RB-1, EV-1, NBR-1, and IR-1: S-1, SE-1, RB-1, EV-1, NBR-1, and IR-1 (thermal conductive particles) described in Table C below. WC-3: Tungsten carbide particles, WC100S (trade name), manufactured by A.L.M.T. Corporation, particle size 10 μm. SiC-1: Silicon carbide particles, SSC-A15 (trade name), manufactured by Shinano Electric Smelting Co., Ltd., particle size 17 μm (hollow particles). B-1: Hollow resin particles, Matsumoto Microsphere MFL-HD60CA (trade name), manufactured by Matsumoto Yushi Pharmaceutical Co., Ltd., plastic microballoons whose surfaces are coated with calcium carbonate powder. Although the values ​​differ depending on the type of backing material sheet (No. 101 to 125, c01 to c18), the particle size of all sheets was within the range of 50 to 70 μm. The particle sizes of the thermally conductive particles and hollow particles are number average particle sizes measured by the following method: The presence of hollow particles in the backing material sheet was confirmed by cutting the backing material sheet with a razor blade and observing the cross section with a tabletop microscope, Miniscope TM4000 (trade name, manufactured by Hitachi High-Technologies Corporation).

[0070] (Measurement of number average particle diameter of particles) The number average particle diameter of the particles was calculated by observing the edge of the backing material sheet in a field of view containing 500 or more particles using a scanning electron microscope (SU8030 (trade name) manufactured by Hitachi High-Technologies Corporation), randomly selecting 500 particles from the field of view, measuring the particle diameters of these particles. For backing material sheets whose edge cannot be observed using a scanning electron microscope, observation was performed using ice-embedding transmission electron microscopy. Ice embedding was performed using a Vitrobot Mark IV (trade name) manufactured by FEI, and 500 particles were randomly selected from the field of view using a transmission electron microscope (JEM-2010 (trade name) manufactured by JEOL Ltd.), and the particle diameters of these particles were measured and calculated. When the particles were not perfectly round, particles with a maximum ratio of vertical to horizontal diameter of 0.7 or more were selected and measured.

[0071] The contents of the resin raw materials, thermally conductive particles (WC-3 and SiC-1), and hollow particles (B-1) are content ratios based on volume. tanδmin (0 to 50°C): Indicates the minimum value of the loss tangent of the resin in the range of 0 to 50°C, measured by the method below. tanδmax (-20 to 110°C): Indicates the maximum value of the loss tangent of the resin in the range of -20 to 110°C, measured by the method below. E' (0 to 50°C): Indicates the evaluation result of the minimum value of the storage modulus of the backing material sheet in the range of 0 to 50°C, measured and evaluated as described above.

[0072] [Measurement of resin loss tangent] (1) Preparation of resin sheet For resin raw materials R-1 to R-23 and PR-1 to PR-10, the base resin and curing agent shown in Table A were weighed out in the compounding ratios shown in Table A, mixed using a centrifugal mixer (product name: Awatori Rentaro Vacuum Type ARV-310, manufactured by Thinky Corporation), molded into a sheet having a length of 30 mm, a width of 5 mm, and a thickness of 0.5 mm, and cured at 100°C for 2 hours, and then cured at 150°C for 2 hours to prepare a resin sheet. For the resin raw materials S-1, SE-1, RB-1, EV-1, NBR-1 and IR-1, the resin raw materials were directly charged into a rotational / revolutionary mixer (trade name: Awatori Rentaro Vacuum Type ARV-310, manufactured by Thinky Corporation), molded into a sheet having a length of 30 mm, a width of 5 mm and a thickness of 0.5 mm, cured at 100 ° C. for 2 hours, and then cured at 150 ° C. for 2 hours to produce a resin sheet. (2) Viscoelasticity Evaluation of Resin Sheet The loss tangent of the produced resin sheet was measured using a dynamic viscoelasticity measuring device itk DVA-225 (trade name, manufactured by IT Measurement Control Co., Ltd.) under the conditions of a grip distance of 20 mm, a heating rate of 2 ° C. / min, a measurement temperature range of -150 ° C. to 250 ° C., and a frequency of 5 Hz.

[0073]

[0074]

[0075]

[0076]

[0077]

[0078] The base agent and curing agent in Table A are as shown in Table B. The blending ratio of the base agent and curing agent is based on mass. A blank in a row of the base agent or curing agent in the table means that the agent is not contained. The functional group equivalent means the mass (g) of the compound per 1 mol of functional group (epoxy group, isocyanato group, or amino group), and is expressed in units of g / mol. The viscosity is measured at 25°C in units of mPa·s. The value was measured using a HAAKE MARS 40 rheometer (trade name, manufactured by Thermo Fisher Scientific) under the following conditions: temperature: 25°C, shear rate: 0.01 / s, sensor: C35 2° / Ti, measurement mode: oscillation mode, frequency: 0.03 Hz. Note that if a material is solid at 25°C, it is described as "solid" in the table. Polymeric MDI stands for polymethylene polyphenyl polyisocyanate, and refers to a mixture of 4,4'-MDI and a high molecular weight polyisocyanate.

[0079] As shown in Table 1, comparative backing material sheets c01 to c03, c05, and c08 to c10 do not satisfy the requirements of the present invention in that the resin loss tangent is less than 0.06 in the temperature range of 0 to 50°C. These comparative backing material sheets c01 to c03, c05, and c08 to c10 had low attenuation rates and poor ultrasonic attenuation. Comparative backing material sheet c06 also did not satisfy the requirements of the present invention in that the resin loss tangent was 1.50 or greater in the temperature range of -20 to 110°C. This comparative backing material sheet c06 also had poor processability. Comparative backing material sheet c04 also did not satisfy the requirements of the present invention in that the resin loss tangent was less than 0.06 in the temperature range of 0 to 50°C and was 1.50 or greater in the temperature range of -20 to 110°C. Comparative backing material sheet No. c04 was poor in ultrasonic attenuation and processability. Comparative backing material sheet No. c07 did not meet the requirements of the present invention in that the storage modulus of the backing material in the temperature range of 0 to 50°C was less than 1000 MPa. Comparative backing material sheet No. c07 also had poor processability. Comparative backing material sheet No. c17 also did not meet the requirements of the present invention in that the resin content in the backing material was 20% by volume. Comparative backing material sheet No. c17 also had poor processability. Comparative backing material sheet No. c18 also did not meet the requirements of the present invention in that the resin content in the backing material was 55% by volume. Comparative backing material sheet No. c18 also had poor processability. Furthermore, comparative backing material sheets Nos. c11 to c16, which use silicone resin, silicone resin-modified epoxy resin, EPDM (ethylene-propylene) rubber, ethylene-vinyl acetate copolymer resin, liquid nitrile rubber, or isoprene rubber, which are known as base materials for backing materials, have a storage modulus of less than 1000 MPa in the range of 0 to 50°C, and in Nos. c11, c12, c15, and c16, the resin loss tangent in the range of 0 to 50°C is less than 0.06, which do not satisfy the requirements of the present invention. These comparative backing material sheets Nos. c11 to c16 were poor in processability.In contrast, it was found that backing material sheets Nos. 101 to 125, which satisfy the requirements of the present invention, are excellent in both ultrasonic attenuation and processability. Furthermore, among backing material sheets Nos. 101 to 125, which satisfy the requirements of the present invention, even those that do not contain hollow particles were excellent in both ultrasonic attenuation and processability, and the effects of the present invention were obtained.

[0080] While the present invention has been described in connection with embodiments thereof, we do not intend to limit our invention to any of the details of the description unless otherwise specified, and believe that the claims should be construed broadly without departing from the spirit and scope of the invention as set forth in the appended claims.

[0081] This application claims priority based on Japanese Patent Application No. 2023-052936, filed on March 29, 2023, the contents of which are incorporated herein by reference as part of the present specification.

[0082] REFERENCE SIGNS LIST 1 acoustic lens 2 acoustic matching layer 3 piezoelectric element layer 4 backing material 7 housing 9 cord 10 ultrasonic probe

Claims

1. A backing material for an ultrasonic probe, comprising thermally conductive particles and a resin, the resin comprising any one of the following (A) to (C): (A) a reaction cured product of an epoxy resin having a polyurethane structure and a polyamine compound, (B) a reaction cured product of an epoxy resin and a polyamine compound, the reaction cured product having a polyether structure, (C) a reaction cured product of a polyisocyanate compound and a polyamine compound; the loss tangent of the resin in the range of 0 to 50°C is 0.06 or more and the loss tangent in the range of -20 to 110°C is less than 1.50, the storage modulus of the backing material in the range of 0 to 50°C is 1000 MPa or more, and the content of the resin in the backing material is 25 to 50 volume %.

2. The backing material of claim 1, wherein the thermally conductive particles include at least one of metal particles and ceramic particles.

3. An ultrasonic probe comprising the backing material of claim 1 or 2.

4. An ultrasonic diagnostic device using the ultrasonic probe according to claim 3.

5. A curable resin composition for forming the backing material according to claim 1 or 2, comprising the thermally conductive particles and any one of the following (a) to (c) as a resin component: (a) a combination of an epoxy resin having a polyurethane structure and a polyamine compound, (b) a combination of an epoxy resin and a polyamine compound, wherein at least one of the epoxy resin and the polyamine compound has a polyether structure, (c) a combination of a polyisocyanate compound and a polyamine compound; and a viscosity of the curable resin composition is 5,000 Pa·s or less at 25°C and a shear rate of 0.01 / s.

Citation Information

Patent Citations

  • Ultrasonic probe, ultrasonic diagnostic device and method for producing backing material

    JP2021062170A

  • Resin composition, acoustic member, ultrasonic transducer, ultrasonic probe and ultrasonic diagnostic apparatus

    JP2022187242A

  • Ultrasonic transducer with acoustic absorber structure

    JP2023502334A

  • High intensity focused ultrasound transducer with acoustic lens

    US20080194967A1