Multi-chip module board
The mounting board design addresses the issue of die marks by using a specific thickness ratio of semiconductor chips to sealing layers and a curable resin composition with colorants, enhancing the visibility and recognition of chip arrangements on the board.
Patent Information
- Application Number
- PCT/JP2024/013038
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional mounting boards face issues with die marks, making it difficult to visually distinguish the external appearance of semiconductor chips and electronic elements, especially when they have different sizes and colors, which complicates the identification of their internal structure.
A mounting board design where the thickness of the semiconductor chip and the sealing layer are within a predetermined ratio (10:1.0 to 10:5.0) and the sealing layer is made of a cured product containing a colorant in a specific proportion (0.60 to 4.0% by mass), using a curable resin composition that includes carbon black and titanium black, to suppress the occurrence of die marks.
The proposed solution effectively suppresses the occurrence of die marks, allowing for better visual recognition of the external appearance and internal structure of the mounting board, even when multiple semiconductor chips of varying sizes and colors are used.
Smart Images

Figure JP2024013038_03102024_PF_FP_ABST
Abstract
Description
Multi-chip module board
[0001] The present invention relates to a mounting board, and more particularly to a mounting board in which a surface of a substrate on which a plurality of semiconductor chips are mounted is sealed with a sealing layer.
[0002] Encapsulation of chip-type devices such as semiconductor elements and electronic components has conventionally been carried out by transfer molding using a powdered epoxy resin composition, or potting, dispensing, printing, etc. using a liquid epoxy resin composition or silicone resin, etc. These encapsulant resin compositions are usually composed of an epoxy resin, a curing agent, a curing accelerator, an inorganic filler, a colorant, etc., and are colored to prevent electrical defects caused by photoexcited currents generated when light strikes the chip and to suppress the occurrence of die marks (see, for example, Patent Document 1).
[0003] In recent years, with the trend toward higher functionality, smaller size, and thinner electronic components, multi-chip modules, which house multiple semiconductor chips and multiple electronic elements in a single package, have been studied and put into practical use as a semiconductor package manufacturing technology. In electronic components such as these multi-chip modules, multiple chip components or electronic components are mounted on a single common substrate and encapsulated with a resin composition. Currently, in order to efficiently manufacture highly integrated devices that require a hollow interior after encapsulation, such as surface acoustic wave (SAW) devices and quartz crystal devices, there is a demand for packaging multiple chip-type devices by encapsulating them together on a substrate.
[0004] In a mounting board that can achieve high functionality and low cost by mounting different types of semiconductor chips and multiple electronic elements as described above, high-density areas where chips such as semiconductor chips and electronic elements are densely arranged and low-density areas where they are sparsely arranged are mixed on a single wiring board, depending on the design (see, for example, Patent Document 2).
[0005] JP 2005-206621 A JP 2014-183085 A
[0006] Conventionally, thin package substrates have had appearance problems such as die marks, which are visible signs of the shape of the internal semiconductor chip after sealing. In particular, in mounting substrates on which multiple semiconductor chips are mounted, as described above, the individual mounted semiconductor chips and electronic elements vary in size and color, so when die marks appear, the mounting positions of the semiconductor chips and electronic elements can be predicted, and in some cases the internal structure of the mounting substrate can be determined just by visually inspecting the exterior.
[0007] Therefore, a primary object of the present invention is to provide a mounting board that can suppress the occurrence of die marks.
[0008] The present inventors focused on the thickness of the semiconductor chip and the thickness of the encapsulating layer and found that, when the thickness of the semiconductor chip and the thickness of the encapsulating layer are within a predetermined range and the colorant contained in the cured product of the curable resin composition that constitutes the encapsulating layer is mixed at a predetermined ratio, the occurrence of die marks can be suppressed even on a mounting substrate. The present invention is based on this finding. That is, the gist of the present invention is as follows.
[0009] [1] A mounting substrate comprising: a substrate; a plurality of semiconductor chips mounted on at least one surface of the substrate; and a sealing layer covering the substrate surface on which the plurality of semiconductor chips are mounted, wherein a thickness of the sealing layer in a thickness direction of the mounting substrate is T, and a distance from an upper surface of each semiconductor chip mounted on the substrate to a surface of the sealing layer is t n , then T:t n [2] A mounting substrate, characterized in that the t is 10:1.0 to 10:5.0, and the sealing layer is made of a cured product of a curable resin composition containing a colorant in a ratio of 0.60 to 4.0 mass %. nThe mounting board according to [1], wherein T is 50 μm or more. [3] The mounting board according to [1] or [2], wherein T is 100 to 500 μm. [4] The mounting board according to any one of [1] to [3], wherein the curable resin composition further contains a thermosetting resin. [5] The mounting board according to any one of [1] to [4], wherein the colorant contains carbon black and titanium black. [6] The mounting board according to any one of [1] to [5], wherein the curable resin composition further contains a thermoplastic resin having a glass transition point of 20°C or less and a weight-average molecular weight of 30,000 or more. [7] The mounting board according to [5], wherein the colorant contains carbon black and titanium black in a ratio of 1:1.1 to 1:7 by mass. [8] The mounting board according to [1] to [6], wherein 3 to 6 semiconductor chips constitute one unit, and the distance between adjacent units is 1 mm or less.
[0010] According to the present invention, by ensuring that the thickness of the semiconductor chip and the thickness of the sealing layer are within a predetermined range and that the colorant contained in the cured product of the curable resin composition that constitutes the sealing layer is mixed in a predetermined ratio, a mounting substrate that can suppress the occurrence of die marks can be obtained.
[0011] Fig. 1 is a front view of a mounting board according to one embodiment of the present invention. Fig. 2 is a cross-sectional view taken along line XX' of the front view of Fig. 1. Fig. 3 is a schematic cross-sectional view of a dry film used to form a sealing layer.
[0012] [Mounting Board] A mounting board comprising a substrate, a plurality of semiconductor chips mounted on at least one surface of the substrate, and a sealing layer covering the substrate surface on which the plurality of semiconductor chips are mounted, wherein the thickness of the sealing layer in the thickness direction of the mounting board is T, and the distance from the top surface of each semiconductor chip mounted on the substrate to the surface of the sealing layer is t n , then T:t n is 10:1.0 to 10:5.0, and the sealing layer is made of a cured product of a curable resin composition containing a colorant in a ratio of 0.60 to 4.0 mass %.
[0013] A mounting board according to one embodiment of the present invention will be described with reference to the drawings. FIG. 1 is a front view of a mounting board according to one embodiment of the present invention, and FIG. 2 is a cross-sectional view taken along line X-X' of the front view of FIG. 1. The mounting board 1 includes a substrate 10 and an encapsulating layer 30 covering the main surface of the substrate 1 on which multiple semiconductor chips 201, 202, ..., 216 are mounted. Three to six (six in FIG. 1 ) of the multiple semiconductor chips 201, 202, ..., 216 constitute a single unit 20A, 20B. Adjacent units 20A and 20B are separated by a predetermined distance. Although not shown, a conductor circuit is patterned on the surface of the substrate 10 in addition to the substrate 10 and the semiconductor chips 201, 202, ..., 216. The encapsulating layer 30 is provided to have a predetermined thickness (T) so as to cover the main surface of the substrate 10. The sealing layer 30 is formed by a distance t from the upper surface of each of the semiconductor chips 211, 212, 213, ... mounted on the main surface of the substrate 10 to the surface of the sealing layer 30. 1 , t 2 , t 3 In the present invention, when viewed in cross section in the thickness direction of the mounting substrate 1, the substrate 10 side of the mounting substrate 1 is referred to as the "bottom" and the sealing layer 30 side is referred to as the "top".
[0014] [Substrate] The substrate used in the mounting board according to the present invention can be a conventionally known one. Examples of the substrate include printed wiring boards and flexible printed wiring boards on which circuits have been formed in advance using copper or the like, as well as copper-clad laminates for high-frequency circuits made of materials such as paper phenol, paper epoxy, glass cloth epoxy, glass polyimide, glass cloth / non-woven cloth epoxy, glass cloth / paper epoxy, synthetic fiber epoxy, fluororesin / polyethylene / polyphenylene ether, polyphenylene oxide / cyanate, and the like, including all grades (FR-4 and the like) of copper-clad laminates, as well as metal substrates, polyimide films, polyethylene terephthalate (PET) films, polyethylene naphthalate (PEN) films, glass substrates, ceramic substrates, and wafers (including wafers before being singulated).
[0015] The thickness of the substrate is not particularly limited, but is preferably 3.0 mm or less, more preferably 2.0 mm or less, even more preferably 1.0 mm or less, and is preferably 0.1 mm or more, more preferably 0.2 mm or more, even more preferably 0.5 mm or more. If the thickness of the substrate is within the above range, the thickness of the entire mounting substrate can be reduced while maintaining strength.
[0016] [Semiconductor Chip] The semiconductor chip used in the mounting substrate of the present invention is not particularly limited in terms of size, thickness, material, color, attachments, function, etc., and any type of conventionally known semiconductor chip can be used. Note that the semiconductor chip here includes not only ordinary semiconductor chips but also surface acoustic wave filter elements (SAW filter elements), crystal oscillator elements, high-frequency elements, acceleration sensors, etc. The mounting substrate of the present invention comprises multiple (at least two or more) semiconductor chips constituting one unit. The number of semiconductor chips included in one unit is not particularly limited as long as it is at least two, but may be 50 or less, preferably 2 to 10. The semiconductor chips included in one unit may all have different shapes or colors, or some of them may have the same shape or color. The distance between adjacent units may be 1 mm or less, or may be 0.4 to 0.7 mm. The distance between adjacent semiconductor chips constituting one unit may be 0.1 to 1 mm, or may be 0.2 to 0.6 mm.
[0017] Furthermore, the semiconductor chip mounted on the substrate does not necessarily need to be arranged so that there is no gap between the substrate and the semiconductor chip; it may be arranged so that a predetermined gap is created between the substrate and the semiconductor chip, for example, as in the case of a SAW filter element.
[0018] [Sealing Layer] The sealing layer is provided to have a predetermined thickness (T) so as to cover the main surface of the substrate. The sealing layer is also provided so that the upper surface of each semiconductor chip mounted on the substrate is spaced a predetermined distance (t nIn the present invention, the thickness of the sealing layer in the thickness direction of the mounting substrate is defined as T, and the distance from the top surface of each semiconductor chip mounted on the substrate to the surface of the sealing layer is defined as t n , then T:t n The thickness of the encapsulating layer is adjusted so that the ratio of T:t is 10:1.0 to 10:5.0. The thickness T of the encapsulating layer refers to the distance from the surface of the substrate on which the semiconductor chip is mounted to the surface of the encapsulating layer. As will be described later, the cured product of the curable resin composition that constitutes the encapsulating layer contains a colorant in a proportion of 0.60 to 4.0 mass %. By adjusting the thickness of the encapsulating layer so that the thickness of the semiconductor chip and the thickness of the encapsulating layer have a predetermined relationship as described above, it is possible to suppress the occurrence of die marks even on mounting substrates where the individual semiconductor chips mounted thereon are different in size and color. n The preferred range is 10:2.0 to 10:4.0.
[0019] The thickness (T) of the sealing layer is adjusted to satisfy the above-mentioned relationship, but in the case of a mounting substrate such as a thin package substrate, the thickness (T) of the sealing layer may be set to 500 μm or less. The thickness (T) of the sealing layer is preferably 100 to 500 μm, more preferably 150 to 400 μm. As described above, each semiconductor chip may have a different shape, but the thickness (T) n The range is preferably 50 μm or more.
[0020] As mentioned above, if there is a gap between the semiconductor chip mounted on the substrate and the substrate, it is preferable that a sealing layer be provided so that the sealing layer does not fill the gap (i.e., so that the sealing layer does not seep in).
[0021] Next, the cured product of the curable resin composition that constitutes the sealing layer will be described. The composition of the curable resin composition used to form the sealing layer is not particularly limited, but as described above, it contains a colorant in a proportion of 0.60 to 4.0 mass %. In addition to the colorant, the curable resin composition usually contains a thermosetting resin, a curing agent, an inorganic filler, etc. The curable resin composition will be described below.
[0022] [Thermosetting Resin] The thermosetting resin is not particularly limited, and known thermosetting resins such as resins having a cyclic ether group and / or a cyclic thioether group, polyisocyanate compounds, blocked isocyanate compounds, amine resins such as melamine resins and benzoguanamine resins and their derivatives, bismaleimide, oxazine, cyclocarbonate compounds, carbodiimide resins, etc. can be used. Among these, epoxy resins can be preferably used.
[0023] The epoxy resin is a resin containing epoxy groups, and any conventionally known epoxy resin can be used. Examples include bifunctional epoxy resins having two epoxy groups per molecule and multifunctional epoxy resins having three or more epoxy groups per molecule. Hydrogenated epoxy resins may also be used. The curable resin composition contains at least one of a semi-solid epoxy resin and a crystalline epoxy resin as the epoxy resin. The semi-solid epoxy resin and the crystalline epoxy resin can be used alone or in combination of two or more. The curable resin composition may also contain a solid epoxy resin or a liquid epoxy resin. In this specification, a solid epoxy resin refers to an epoxy resin that is solid at 40°C, a semi-solid epoxy resin refers to an epoxy resin that is solid at 20°C and liquid at 40°C, and a liquid epoxy resin refers to an epoxy resin that is liquid at 20°C.
[0024] Examples of semi-solid epoxy resins include bisphenol A type epoxy resins such as Epicron 860, Epicron 900-IM, Epicron EXA-4816, and Epicron EXA-4822 manufactured by DIC Corporation, Araldite AER280 manufactured by Asahi Chiba Corporation, Epotohto YD-134 manufactured by Tohto Kasei Co., Ltd., jER834 and jER872 manufactured by Mitsubishi Chemical Corporation, and ELA-134 manufactured by Sumitomo Chemical Co., Ltd.; naphthalene type epoxy resins such as Epicron HP-4032 manufactured by DIC Corporation; and phenol novolac type epoxy resins such as Epicron N-740 manufactured by DIC Corporation.
[0025] The semi-solid epoxy resin preferably contains at least one selected from the group consisting of bisphenol A epoxy resins, naphthalene epoxy resins, and phenol novolac epoxy resins. By including the semi-solid epoxy resin, the cured product has a high glass transition temperature (Tg), a low CTE, and excellent crack resistance.
[0026] Examples of crystalline epoxy resins that can be used include crystalline epoxy resins having a biphenyl structure, a sulfide structure, a phenylene structure, a naphthalene structure, etc. Biphenyl-type epoxy resins are available, for example, as jER YX4000, jER YX4000H, jER YL6121H, jER YL6640, and jER YL6677 manufactured by Mitsubishi Chemical Corporation. Diphenyl sulfide-type epoxy resins are available, for example, as Epotohto YSLV-120TE manufactured by Tohto Kasei Co., Ltd. Phenylene-type epoxy resins are available, for example, as Epotohto YDC-1312 manufactured by Tohto Kasei Co., Ltd. Naphthalene-type epoxy resins are available, for example, as EPICLON HP-4032, EPICLON HP-4032D, and EPICLON HP-4700 manufactured by DIC Corporation. Furthermore, as the crystalline epoxy resin, Epotohto YSLV-90C manufactured by Tohto Kasei Co., Ltd. and TEPIC-S (triglycidyl isocyanurate) manufactured by Nissan Chemical Industries, Ltd. can also be used.
[0027] Examples of solid epoxy resins include naphthalene-type epoxy resins such as HP-4700 (naphthalene-type epoxy resin) manufactured by DIC Corporation, EXA4700 (tetrafunctional naphthalene-type epoxy resin) manufactured by DIC Corporation, and NC-7000 (naphthalene skeleton-containing multifunctional solid epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; epoxidized products of condensates of phenols and aromatic aldehydes having a phenolic hydroxyl group (trisphenol-type epoxy resins) such as EPPN-502H (trisphenol epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; and Epicron HP-7200H (dicyclopentadiene skeleton-containing multifunctional solid epoxy resin) manufactured by DIC Corporation. biphenyl aralkyl type epoxy resins such as NC-3000H (biphenyl skeleton-containing polyfunctional solid epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; biphenyl / phenol novolac type epoxy resins such as NC-3000L manufactured by Nippon Kayaku Co., Ltd.; novolac type epoxy resins such as Epiclon N660, Epiclon N690, and N770 manufactured by DIC Corporation and EOCN-104S manufactured by Nippon Kayaku Co., Ltd.; phosphorus-containing epoxy resins such as TX0712 manufactured by Nippon Steel & Sumikin Chemical Co., Ltd.; and tris(2,3-epoxypropyl)isocyanurate such as TEPIC manufactured by Nissan Chemical Industries, Ltd. By including a solid epoxy resin, the glass transition temperature of the cured product is increased, resulting in excellent heat resistance.
[0028] Examples of liquid epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AF type epoxy resins, phenol novolac type epoxy resins, tert-butyl-catechol type epoxy resins, glycidylamine type epoxy resins, aminophenol type epoxy resins, alicyclic epoxy resins, etc. By including a liquid epoxy resin, the dry film has excellent flexibility.
[0029] The total amount of the semi-solid epoxy resin and the crystalline epoxy resin is preferably 5 to 40 mass % based on the total amount of the epoxy resin, and more preferably 10 to 30 mass %. When the amount is within this range, the curable resin composition has excellent tackiness and flexibility when formed into a dry film.
[0030] In addition to epoxy resins, the thermoplastic resin may include known and commonly used thermosetting resins such as isocyanate compounds, blocked isocyanate compounds, amino resins, benzoxazine resins, carbodiimide resins, cyclocarbonate compounds, polyfunctional oxetane compounds, and episulfide resins.
[0031] [Curing Agent] When using the above-mentioned thermosetting resin, the curable resin composition preferably contains a curing agent. Examples of the curing agent include a compound having a phenolic hydroxyl group, a polycarboxylic acid and its acid anhydride, a compound having a cyanate ester group, a compound having an active ester group, a compound having a maleimide group, and an alicyclic olefin polymer. The curing agent can be used alone or in combination of two or more.
[0032] The curable resin composition preferably contains at least one of a compound having a phenolic hydroxyl group, a compound having an active ester group, a compound having a cyanate ester group, and a compound having a maleimide group. By using a compound having a phenolic hydroxyl group and a compound having an active ester group, a cured product with excellent adhesion to low-roughness substrates and circuits can be obtained. In addition, by using a cyanate ester, the Tg of the cured product is increased, improving heat resistance, and by using a compound having a maleimide group, the Tg of the cured product is increased, improving heat resistance, and reducing the CTE.
[0033] Examples of the compound having a phenolic hydroxyl group that can be used include conventionally known compounds such as phenol novolac resins, alkylphenol novolac resins, bisphenol A novolac resins, dicyclopentadiene-type phenolic resins, Xylok-type phenolic resins, terpene-modified phenolic resins, cresol / naphthol resins, polyvinylphenols, phenol / naphthol resins, α-naphthol skeleton-containing phenolic resins, triazine skeleton-containing cresol novolac resins, biphenylaralkyl-type phenolic resins, and Xylok-type phenolic novolac resins.
[0034] Among compounds having a phenolic hydroxyl group, those having a hydroxyl group equivalent of 100 g / eq. or more are preferred. Examples of compounds having a phenolic hydroxyl group with a hydroxyl group equivalent of 100 g / eq. or more include dicyclopentadiene skeleton phenol novolac resin (GDP series, manufactured by Gun-ei Chemical Co., Ltd.), Zylok type phenol novolac resin (MEH-7800, manufactured by Meiwa Chemical Industry Co., Ltd.), biphenyl aralkyl type novolac resin (MEH-7851, manufactured by Meiwa Chemical Industry Co., Ltd.), naphthol aralkyl type curing agent (SN series, manufactured by Nippon Steel & Sumitomo Metal Corporation), triazine skeleton-containing cresol novolac resin (LA-3018-50P, manufactured by DIC Corporation), and triazine skeleton-containing phenol novolac resin (LA-705N, manufactured by DIC Corporation).
[0035] Among compounds having a phenolic hydroxyl group, those having a hydroxyl group equivalent of 100 g / eq. or more are preferred. Examples of compounds having a phenolic hydroxyl group with a hydroxyl group equivalent of 100 g / eq. or more include dicyclopentadiene skeleton phenol novolac resin (GDP series, manufactured by Gun-ei Chemical Co., Ltd.), Zylok type phenol novolac resin (MEH-7800, manufactured by Meiwa Chemical Industry Co., Ltd.), biphenyl aralkyl type novolac resin (MEH-7851, manufactured by Meiwa Chemical Industry Co., Ltd.), naphthol aralkyl type curing agent (SN series, manufactured by Nippon Steel & Sumitomo Metal Corporation), triazine skeleton-containing cresol novolac resin (LA-3018-50P, manufactured by DIC Corporation), and triazine skeleton-containing phenol novolac resin (LA-705N, manufactured by DIC Corporation).
[0036] Commercially available compounds having a cyanate ester group include phenol novolac-type multifunctional cyanate ester resin (PT30S, manufactured by Lonza Japan), a prepolymer in which part or all of bisphenol A dicyanate has been triazinated to form a trimer (BA230S75, manufactured by Lonza Japan), and a dicyclopentadiene structure-containing cyanate ester resin (DT-4000, DT-7000, manufactured by Lonza Japan).
[0037] The compound having an active ester group is preferably a compound having two or more active ester groups in one molecule. Compounds having an active ester group can generally be obtained by a condensation reaction between a carboxylic acid compound and a hydroxy compound. Among these, compounds having an active ester group obtained using a phenol compound or a naphthol compound as the hydroxy compound are preferred. Examples of phenol compounds or naphthol compounds include hydroquinone, resorcinol, bisphenol A, bisphenol F, bisphenol S, phenolphthalene, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucinol, benzenetriol, dicyclopentadienyldiphenol, and phenol novolak. The compound having an active ester group may also be a naphthalenediol alkyl / benzoic acid type.
[0038] Commercially available compounds having an active ester group include dicyclopentadiene-type diphenol compounds such as HPC8000-65T (manufactured by DIC Corporation), HPC8100-65T (manufactured by DIC Corporation), and HPC8150-65T (manufactured by DIC Corporation).
[0039] The compound having a maleimide group is a compound having a maleimide skeleton, and any of the conventionally known compounds can be used. The compound having a maleimide group preferably has two or more maleimide skeletons, and examples thereof include N,N'-1,3-phenylenedimaleimide, N,N'-1,4-phenylenedimaleimide, N,N'-4,4-diphenylmethane bismaleimide, 1,2-bis(maleimide)ethane, 1,6-bismaleimidohexane, 1,6-bismaleimido-(2,2,4-trimethyl)hexane, and 2,2'-bis-[4-(4-maleimidophenoxy)phenyl]propane. More preferably, the oligomer is at least one of bismaleimide, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, bisphenol A diphenyl ether bismaleimide, polyphenylmethane maleimide, and oligomers thereof, as well as diamine condensates having a maleimide skeleton. The oligomer is an oligomer obtained by condensing a compound having a maleimide group, which is a monomer among the above-mentioned compounds having a maleimide group.
[0040] Commercially available compounds having a maleimide group include BMI-1000 (4,4'-diphenylmethane bismaleimide, manufactured by Daiwa Chemical Industry Co., Ltd.), BMI-2300 (phenylmethane bismaleimide, manufactured by Daiwa Chemical Industry Co., Ltd.), BMI-3000 (m-phenylene bismaleimide, manufactured by Daiwa Chemical Industry Co., Ltd.), BMI-5100 (3,3'-dimethyl-5,5'-dimethyl-4,4'-diphenylmethane bismaleimide, manufactured by Daiwa Chemical Industry Co., Ltd.), BMI-7000 (4-methyl-1,3-phenylene bismaleimide, manufactured by Daiwa Chemical Industry Co., Ltd.), and BMI-TMH ((1,6-bismaleimide-2,2,4-trimethyl)hexane, manufactured by Daiwa Chemical Industry Co., Ltd.).
[0041] The amount of the curing agent to be added is preferably 20 to 100 parts by mass, and more preferably 25 to 90 parts by mass, per 100 parts by mass of the thermosetting resin.
[0042] [Curing Accelerator] The curable resin composition may contain a curing accelerator in combination with a curing agent. The curing accelerator accelerates the thermosetting reaction and is used to further improve properties such as adhesion, chemical resistance, and heat resistance. Specific examples of such curing accelerators include imidazole and its derivatives; guanamines such as acetoguanamine and benzoguanamine; polyamines such as diaminodiphenylmethane, m-phenylenediamine, m-xylylenediamine, diaminodiphenylsulfone, dicyandiamide, urea, urea derivatives, melamine, and polybasic hydrazides; organic acid salts and / or epoxy adducts thereof; amine complexes of boron trifluoride; triazine derivatives such as ethyldiamino-S-triazine, 2,4-diamino-S-triazine, and 2,4-diamino-6-xylyl-S-triazine; amines such as trimethylamine, triethanolamine, N,N-dimethyloctylamine, N-benzyldimethylamine, pyridine, N-methylmorpholine, hexa(N-methyl)melamine, 2,4,6-tris(dimethylaminophenol), tetramethylguanidine, and m-aminophenol; polyvinylphenol, brominated polyvinylphenol, and phenol novolak. Examples of suitable curing accelerators include polyphenols such as alkylphenol novolak and alkylphenol novolak; organic phosphines such as tributylphosphine, triphenylphosphine, and tris-2-cyanoethylphosphine; phosphonium salts such as tri-n-butyl(2,5-dihydroxyphenyl)phosphonium bromide and hexadecyltributylphosphonium chloride; quaternary ammonium salts such as benzyltrimethylammonium chloride and phenyltributylammonium chloride; the above-mentioned polybasic acid anhydrides; photocationic polymerization catalysts such as diphenyliodonium tetrafluoroborate, triphenylsulfonium hexafluoroantimonate, and 2,4,6-triphenylthiopyrylium hexafluorophosphate; styrene-maleic anhydride resins; equimolar reactants of phenyl isocyanate and dimethylamine, equimolar reactants of organic polyisocyanates such as tolylene diisocyanate and isophorone diisocyanate and dimethylamine, and metal catalysts. Among these curing accelerators, phosphonium salts are preferred because of their ability to provide BHAST resistance.
[0043] The curing accelerator can be used alone or in combination of two or more. The use of a curing accelerator is not essential, but when it is particularly desired to accelerate curing, it can be used in an amount of preferably 0.01 to 5 parts by mass per 100 parts by mass of the epoxy resin. In the case of a metal catalyst, the amount is preferably 10 to 550 ppm, more preferably 25 to 200 ppm, calculated as metal per 100 parts by mass of the compound having a cyanate ester group.
[0044] [Colorant] The curable resin composition used to form the sealing layer contains a colorant in a proportion of 0.60 to 4.0 mass% in terms of solid content. When the colorant proportion is 0.60 mass% or more, the occurrence of die marks can be suppressed by adjusting the thickness of the sealing layer. Furthermore, when the colorant proportion is less than 4.0 mass%, the dispersibility of the curable resin composition can be improved. The preferred blending proportion of the colorant is 0.60 to 2.5 mass%.
[0045] As the colorant, known colorants used in conventional encapsulants can be used, such as phthalocyanine blue, phthalocyanine green, iodine green, disazo yellow, crystal violet, carbon black, titanium black, naphthalene black, etc. Among these, carbon black and titanium black can be preferably used from the viewpoint of suppressing the occurrence of die marks.
[0046] In the present invention, it is preferable to use carbon black and titanium black in combination as colorants. When both are used in combination, the carbon black and titanium black are contained in a ratio of 1:1.1 to 1:7 by mass, more preferably 1:2 to 1:4 by mass.
[0047] [Other Resin Components] The curable resin composition used to form the sealing layer may further contain a thermoplastic resin to improve mechanical strength. The thermoplastic resin is preferably soluble in a solvent. When the thermoplastic resin is soluble in a solvent, the flexibility of the dry film is improved, and cracking and powdering can be suppressed. Examples of the thermoplastic resin include thermoplastic polyhydroxypolyether resins, phenoxy resins which are condensates of epichlorohydrin and various bifunctional phenolic compounds, or phenoxy resins in which the hydroxyl groups of the hydroxyether moieties present in the skeleton are esterified using various acid anhydrides or acid chlorides, polyvinyl acetal resins, polyamide resins, polyamideimide resins, and block copolymers. The thermoplastic resins may be used alone or in combination of two or more.
[0048] The curable resin composition may contain, for example, a thermoplastic resin having a glass transition temperature of 20°C or lower and a weight average molecular weight of 30,000 or higher. Since the higher the weight average molecular weight of the polymer resin, the greater the effect of preventing the sedimentation of the inorganic filler, the weight average molecular weight is preferably 100,000 or higher, and more preferably 200,000 or higher. The upper limit is, for example, 1,000,000 or lower.
[0049] Examples of the thermoplastic resin include polymer resins having one or more skeletons selected from a butadiene skeleton, an amide skeleton, an imide skeleton, an acetal skeleton, a carbonate skeleton, an ester skeleton, a urethane skeleton, an acrylic skeleton, and a siloxane skeleton. Examples thereof include polymer resins having a butadiene skeleton ("G-1000", "G-3000", "GI-1000", "GI-3000" manufactured by Nippon Soda Co., Ltd., "R-45EPI" manufactured by Idemitsu Petrochemical Co., Ltd., "PB3600" and "Epofriend AT501" manufactured by Daicel Chemical Industries, Ltd., and "Ricon130", "Ricon142", "Ricon150", "Ricon657", and "Ricon130MA" manufactured by Cray Valley Chemical Industries, Ltd.), polymer resins having a butadiene skeleton and a polyimide skeleton (those described in JP 2006-37083 A), and polymer resins having an acrylic skeleton ("SG-P3", "SG-600LB", "SG-280", "SG-790", and "SG-K2" manufactured by Nagase ChemteX Corporation, and "SN-50", "AS-3000E", and "ME-2000" manufactured by Negami Chemical Industrial Co., Ltd.).
[0050] From the viewpoint of flatness of the cured product, the thermoplastic resin is preferably an acrylic copolymer having a glass transition point of 20°C or less and a weight average molecular weight of 200,000 or more. Also, from the viewpoint of adhesion to biaxially oriented polypropylene film (OPP) and adhesion to low-roughness substrates and circuits, the thermoplastic resin is preferably an acrylic copolymer having a glass transition point of -5 to 15°C and a weight average molecular weight of 200,000 to 500,000.
[0051] The acrylic acid ester copolymer may have a functional group, such as a carboxyl group, a hydroxyl group, an epoxy group, or an amide group. The acrylic acid ester copolymer preferably has an epoxy group, and more preferably has an epoxy group and an amide group. The presence of an epoxy group can suppress warping of the cured product.
[0052] Examples of the acrylic acid ester copolymer include Teisan Resin SG-70L, SG-708-6, WS-023 EK30, SG-P3, SG-80H, SG-280 EK23, SG-600TEA, and SG-790, manufactured by Nagase ChemteX Corp. The acrylic acid ester copolymer may be obtained by synthesis, and examples of the synthesis method include the synthesis method described in JP 2016-102200 A.
[0053] The thermoplastic resin may be used alone or in combination of two or more. The blending amount of the polymer is preferably 0.5 to 10 mass %, more preferably 1.0 to 7.0 mass %, even more preferably 2.0 to 7.0 mass %, and particularly preferably 4.0 to 7.0 mass %, based on the total solid content of the composition.
[0054] The amount of the thermoplastic resin blended is preferably 0.5 to 20 mass %, more preferably 0.5 to 10 mass %, based on the total solid content of the curable resin composition. When the amount of the thermoplastic resin blended is within the above range, a uniform roughened surface state is easily obtained, and as a result, the occurrence of die marks can be suppressed.
[0055] The curable resin composition can contain rubber particles as needed. Examples of such rubber particles include polybutadiene rubber, polyisopropylene rubber, urethane-modified polybutadiene rubber, epoxy-modified polybutadiene rubber, acrylonitrile-modified polybutadiene rubber, carboxyl-modified polybutadiene rubber, carboxyl- or hydroxyl-modified acrylonitrile-butadiene rubber, and crosslinked rubber particles thereof, core-shell type rubber particles, etc., and one type can be used alone or two or more types can be used in combination. These rubber particles are added to improve the flexibility of the resulting cured film, improve crack resistance, enable surface roughening treatment with an oxidizing agent, and improve adhesion strength with copper foil, etc.
[0056] The average particle size of the rubber-like particles is preferably in the range of 0.005 to 1 μm, more preferably in the range of 0.2 to 1 μm. The average particle size of the rubber-like particles in the present invention can be determined using a laser diffraction particle size distribution analyzer. For example, the rubber-like particles are uniformly dispersed in an appropriate organic solvent using ultrasound or the like, and a particle size distribution of the rubber-like particles is created on a mass basis using a Nanotrac wave manufactured by Nikkiso Co., Ltd., and the median diameter is used as the average particle size.
[0057] The amount of rubber particles is preferably 0.5 to 10% by mass, more preferably 1 to 5% by mass, based on the total solid content of the curable resin composition. When the amount is 0.5% by mass or more, crack resistance is obtained and adhesive strength with a conductor pattern or the like can be improved. When the amount is 10% by mass or less, the coefficient of thermal expansion (CTE) decreases and the glass transition temperature increases, improving curing characteristics.
[0058] [Inorganic Filler] The curable resin composition may contain an inorganic filler as needed. The incorporation of an inorganic filler can suppress cure shrinkage of the resulting cured product and improve thermal properties such as adhesion, hardness, and crack resistance by matching the thermal strength of the insulating layer with that of a conductor layer such as copper surrounding the insulating layer. Conventionally known inorganic fillers can be used as the inorganic filler, and are not limited to specific ones. Examples of inorganic fillers include silica (e.g., barium sulfate, barium titanate, amorphous silica, crystalline silica, fused silica, and spherical silica), talc, clay, Neuburg silica particles, boehmite, magnesium carbonate, calcium carbonate, titanium oxide, aluminum oxide, aluminum hydroxide, silicon nitride, aluminum nitride, and calcium zirconate, as well as extender pigments such as copper, tin, zinc, nickel, silver, palladium, aluminum, iron, cobalt, gold, and platinum. Spherical particles are preferred for the inorganic filler. Among these, silica is preferred, as it suppresses cure shrinkage of the cured product of the curable composition, lowers the CTE, and improves properties such as adhesion and hardness. Furthermore, inorganic fillers with a high specific gravity, such as alumina, generally have a high sedimentation rate, but can be used advantageously in the present invention because sedimentation can be suppressed. The average particle size (median diameter, D50) of the inorganic filler is preferably 0.01 to 10 μm. From the viewpoint of slit processability, silica with an average particle size of 0.01 to 3 μm is preferred as the inorganic filler. In this specification, the average particle size of the inorganic filler refers to the average particle size including not only the particle size of primary particles but also the particle size of secondary particles (aggregates). The average particle size can be determined using a laser diffraction particle size distribution analyzer. An example of a measuring device using the laser diffraction method is the Nanotra Wave manufactured by Nikkiso Co., Ltd.
[0059] The inorganic filler may be surface-treated. The surface treatment may include surface treatment with a coupling agent or surface treatment without introducing an organic group, such as alumina treatment. The surface treatment method for the inorganic filler is not particularly limited, and any known or commonly used method may be used. The surface of the inorganic filler may be treated with a surface treatment agent having a curable reactive group, for example, a coupling agent having a curable reactive group as an organic group.
[0060] The surface treatment of the inorganic filler is preferably a surface treatment with a coupling agent. Examples of coupling agents that can be used include silane-based, titanate-based, aluminate-based, and zircoaluminate-based coupling agents. Among these, silane-based coupling agents are preferred. Examples of such silane-based coupling agents include vinyltrimethoxysilane, vinyltriethoxysilane, N-(2-aminomethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-anilinopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane. These can be used alone or in combination. It is preferable that these silane-based coupling agents are immobilized on the surface of the inorganic filler in advance by adsorption or reaction. Here, the amount of the coupling agent to be treated with respect to 100 parts by mass of the inorganic filler is, for example, 0.5 to 10 parts by mass.
[0061] The curable reactive group is preferably a thermosetting reactive group. Examples of the thermosetting reactive group include a hydroxyl group, a carboxyl group, an isocyanate group, an amino group, an imino group, an epoxy group, an oxetanyl group, a mercapto group, a methoxymethyl group, a methoxyethyl group, an ethoxymethyl group, an ethoxyethyl group, and an oxazoline group. Among these, at least one of an amino group and an epoxy group is preferred. The surface-treated inorganic filler may have a photocurable reactive group in addition to the thermosetting reactive group.
[0062] The surface-treated inorganic filler may be contained in the curable resin composition in a surface-treated state. The inorganic filler and the surface treatment agent may be separately blended into the curable resin composition forming the sealing layer to surface-treat the inorganic filler in the composition. However, it is preferable to blend a pre-surface-treated inorganic filler. Blending a pre-surface-treated inorganic filler can prevent a decrease in crack resistance, etc., due to the surface treatment agent that may remain in the surface treatment if blended separately. When performing pre-surface treatment, it is preferable to blend a pre-dispersion in which the inorganic filler is pre-dispersed in a solvent or curable resin. The surface-treated inorganic filler is pre-dispersed in a solvent and the pre-dispersion is blended into the composition. Alternatively, it is more preferable to pre-disperse a surface-untreated inorganic filler in a solvent, thoroughly surface-treat it, and then blend the pre-dispersion into the composition.
[0063] The inorganic filler may be blended with the epoxy resin or the like in a powder or solid state, or may be mixed with a solvent or dispersant to form a slurry and then blended with the epoxy resin or the like.
[0064] The inorganic filler may be used alone or as a mixture of two or more. The amount of the inorganic filler is preferably 10 to 90 mass %, more preferably 50 to 90 mass %, and even more preferably 60 to 90 mass %, based on the total solid content of the curable resin composition. When the amount of the inorganic filler is 10 mass % or more, thermal expansion is suppressed and heat resistance is improved, while when the amount is 90 mass % or less, the occurrence of cracks can be suppressed.
[0065] The problems of adhesion of the protective film and sedimentation of the inorganic filler are particularly pronounced when the content of the inorganic filler is high. In the present invention, particularly excellent effects can be obtained when the amount of inorganic filler is high, for example, when the amount is 50 mass% or more based on the total solid content of the curable resin composition. Furthermore, when the amount is 70 mass% or more, sedimentation of the inorganic filler is particularly pronounced, but according to the present invention, sedimentation of the inorganic filler is excellently suppressed.
[0066] [Organic Solvent] The curable resin composition described above may contain an organic solvent. When forming a dry film as described below, the viscosity of the curable resin composition can be adjusted to an appropriate range to improve coatability. The organic solvent is not particularly limited, and examples thereof include ketones, aromatic hydrocarbons, glycol ethers, glycol ether acetates, esters, alcohols, aliphatic hydrocarbons, and petroleum-based solvents. Specific examples include ketones such as methyl ethyl ketone, cyclohexanone, methyl butyl ketone, and methyl isobutyl ketone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; ethyl acetate, butyl acetate, isobutyl acetate, ethylene glycol monomethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; ethyl acetate, butyl acetate, isobutyl acetate, ethylene glycol monomethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; ethyl acetate, butyl acetate, isobutyl acetate, ethylene glycol monomethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; ethyl acetate, butyl acetate, isobutyl acetate, ethyl ... Examples of suitable solvents include esters such as propylene glycol monoethyl ether acetate, dipropylene glycol methyl ether acetate, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, and propylene glycol butyl ether acetate; alcohols such as ethanol, propanol, 2-methoxypropanol, n-butanol, isobutyl alcohol, isopentyl alcohol, ethylene glycol, and propylene glycol; aliphatic hydrocarbons such as octane and decane; petroleum solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha, as well as N,N-dimethylformamide (DMF), tetrachloroethylene, and turpentine. Alternatively, organic solvents such as Swazol 1000 and Swazol 1500 manufactured by Maruzen Petrochemical Co., Ltd., Solvesso 100 and Solvesso 150 manufactured by Standard Oil Osaka Sales Co., Ltd., Solvent #100 and Solvent #150 manufactured by Sankyo Chemical Co., Ltd., Shellsol A100 and Shellsol A150 manufactured by Shell Chemicals Japan, and Ipzol 100 and Ipzol 150 manufactured by Idemitsu Kosan Co., Ltd. may be used.The organic solvent may be used alone or in combination of two or more.
[0067] The amount of residual solvent in the curable resin composition is preferably 0.5 to 7.0% by mass. When the residual solvent is 7.0% by mass or less, bumping during thermal curing is suppressed, resulting in better surface flatness. Furthermore, excessively low melt viscosity that causes the resin to flow can be suppressed, resulting in better flatness. When the residual solvent is 0.5% by mass or more, the flowability during lamination is good, resulting in better flatness and embeddability.
[0068] [Other Components] If necessary, the curable resin composition may further contain conventionally known additives such as asbestos, Orben, Bentone, finely divided silica, etc., silicone-based, fluorine-based, polymer-based, etc. antifoaming agents and / or leveling agents, adhesion promoters such as thiazole-based, triazole-based, silane coupling agents, etc., flame retardants, titanate-based, and aluminum-based.
[0069] [Dry Film] The encapsulating layer is preferably formed using a dry film having a resin layer made of a curable resin composition. Figure 3 is a cross-sectional schematic diagram of a dry film used to form the encapsulating layer. The dry film 40 includes a first film 401, a resin layer 402 provided on one side of the first film, and a second film 403 provided on the opposite side of the resin layer 402 from the first film 401, so as to contact the resin layer 402. An intermediate layer (not shown) may be provided between the first film 401 and the resin layer 402. When using the dry film 40, the second film 403 is peeled off to expose the resin layer 402, and the resin layer 402 of the dry film 40 is laminated to the main surface of a substrate on which a semiconductor chip or the like is mounted. That is, the second film 403 is provided to prevent dust and the like from adhering to the surface of the resin layer 402 and to facilitate handling of the dry film 40, and is intended to be peeled off when the dry film 40 is used.
[0070] The first film refers to a film that is adhered to at least the resin layer when the dry film is laminated onto a substrate or other base material by heating or the like so that the resin layer side made of the curable resin composition formed on the dry film is in contact with the base material. The first film may be peeled off from the resin layer in a step after lamination.
[0071] The first film can be any known film without particular limitation, and examples of suitable films include polyester films such as polyethylene terephthalate and polyethylene naphthalate, and films made of thermoplastic resins such as polyimide films, polyamideimide films, polypropylene films, and polystyrene films. Among these, polyester films are preferred from the viewpoints of heat resistance, mechanical strength, ease of handling, etc. A laminate of these films can also be used as the first film.
[0072] The surface of the first film on which the resin layer is to be formed may be subjected to a release treatment. For example, the release treatment can be performed by applying a coating liquid prepared by dissolving or dispersing a release agent such as waxes, silicone wax, or silicone-based resin in an appropriate solvent to the surface of the first film by a known coating method such as roll coating, spray coating, gravure printing, or screen printing, and then drying the coating liquid.
[0073] The thickness of the first film is not particularly limited, but can be, for example, 10 μm to 150 μm.
[0074] The resin layer provided on one side of the first film is made of the curable resin composition described above. The curable resin composition is applied to a uniform thickness on the surface of the first film using a comma coater, blade coater, lip coater, rod coater, squeeze coater, reverse coater, transfer roll coater, gravure coater, spray coater, or the like, and the resin layer can be formed by drying the applied film at a temperature of 50 to 130°C for 1 to 30 minutes. There are no particular restrictions on the thickness of the applied film, but the thickness after drying is appropriately selected from the range of 5 to 40 μm, preferably 10 to 35 μm.
[0075] As the second film, for example, a polyester film, a polyethylene film, a polytetrafluoroethylene film, a polypropylene film, surface-treated paper, etc. can be used, but among these, a polypropylene film can be preferably used.
[0076] It is preferable to select a material such that the adhesive strength between the second film and the resin layer is smaller than the adhesive strength between the first film and the resin layer. In addition, to make it easier to peel off the second film when using the dry film, the surface of the second film that comes into contact with the resin layer may be subjected to the above-mentioned release treatment.
[0077] The thickness of the second film is not particularly limited, but is generally selected appropriately within the range of 10 to 60 μm depending on the application.
[0078] [Method for Manufacturing Mounted Substrate] The second film 403 of the dry film 40 shown in Figure 3 is peeled off to expose the resin layer 402, which is then laminated under pressure and heat using a vacuum laminator or the like onto the main surface of a substrate on which multiple semiconductor chips and the like are mounted. By using a vacuum laminator, the resin layer 402 adheres tightly to the substrate, making it difficult for air bubbles to be trapped even if there are recesses between the semiconductor chips mounted on the substrate surface, and allowing the formation of a smooth sealing layer. The pressure conditions are preferably approximately 0.1 to 2.0 MPa, and the heating conditions are preferably 40 to 120°C.
[0079] After the resin layer 403 is cured, the first film 401 is peeled off to form the sealing layer 30. The resin layer 403 is preferably cured by heat and pressure molding. Heat and pressure molding can be performed using known methods such as a vacuum laminator or a vacuum press. The temperature during heat and pressure molding is 60 to 130°C, and the pressure is 20 kg / cm. 2 The molding time is preferably within 180 seconds. Then, the sealing layer 30 is thermally cured to seal the product. The thermal curing is performed at 100 to 200° C. for about 30 to 180 minutes.
[0080] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples. In the following, "parts" and "%" are all by mass unless otherwise specified.
[0081] <Preparation of Curable Resin Composition> According to the formulation shown in Table 1 below, the components were mixed and stirred, and then kneaded using a three-roll mill to prepare two types of curable resin compositions, A and B. The values in the table indicate parts by mass, and components other than the solvent indicate the amount of solids.
[0082]
[0083] In Table 1, *1 to *11 represent the following components: *1: Bisphenol A epoxy resin (manufactured by Mitsubishi Chemical Corporation) *2: Phenol novolac epoxy resin (manufactured by DIC Corporation) *3: Phenol novolac epoxy resin (manufactured by DIC Corporation) *4: Phenol novolac resin (manufactured by UBE Corporation) *5: Leveling agent (manufactured by BYK Japan KK) *6: Silane coupling agent (manufactured by Shin-Etsu Silicones Co., Ltd.) *7: Spherical silica (manufactured by Admatechs Co., Ltd.) *8: Acrylic acid ester copolymer (functional group: epoxy group, Tg = 12°C, Mw = 850,000, manufactured by Nagase ChemteX Corporation) *9: Imidazole epoxy curing agent (manufactured by Shikoku Chemicals Co., Ltd.) *10: Titanium black (manufactured by Ako Chemicals Co., Ltd.) *11: Carbon black (manufactured by Resino Color Kogyo Co., Ltd.) *12: Cyclohexanone (manufactured by Taishin Chemical Co., Ltd.)
[0084] <Preparation of Dry Film> The amount of solvent was adjusted so that the prepared curable resin composition A had a viscosity of 0.5 to 20 dPa·s (rotational viscometer 5 rpm, 25°C), and each was applied using a bar coater to a release PET film (TN201, manufactured by Toyobo Co., Ltd., thickness 50 μm, size 30 cm × 30 cm) so that the thickness of the resin layer after drying would be 200 μm. Next, the film was dried at 90°C for 15 minutes in a hot air circulation drying oven to form a resin layer on the release PET film. Subsequently, a fresh airless OPP (Alphan FG-201, manufactured by Oji F-Tex Co., Ltd.) was adhered to the surface of the formed resin layer using a roll laminator to prepare dry film 1 having a resin layer thickness of 200 μm.
[0085] Dry film 2 having a resin layer thickness of 150 μm was also prepared in the same manner as above, except that the amount of curable resin composition A applied was adjusted so that the thickness of the resin layer after drying would be 150 μm.
[0086] Further, dry film 3 having a resin layer thickness of 240 μm was prepared in the same manner as above, except that the amount of curable resin composition A applied was adjusted so that the thickness of the resin layer after drying would be 240 μm.
[0087] Dry film 4 having a resin layer thickness of 200 μm was prepared in the same manner as dry film 1, except that curable resin composition A was changed to curable resin composition B.
[0088] Two dry films 4 were also prepared, the OPP and carrier film were peeled off from each dry film, and the two resin layers were bonded together at 80°C using a roll laminator to produce a dry film 5 with a resin layer thickness of 400 μm.
[0089] [Example 1] Three types of chips, 190 μm, 200 μm, and 220 μm thick, were mounted at 0.5 mm intervals with a gap of 10 to 15 μm from the substrate. A 0.4 mm thick FR-4 substrate was formed with a cured coating of a 0.2 mm thick solder resist ink (PSR-4000 AUS308, manufactured by Taiyo Ink Mfg. Co., Ltd.). The fresh airless OPP was peeled off to expose the resin layer. Dry film 1 was then laminated using a vacuum laminator at a temperature of 55°C, a pressure of 0.5 MPa, and for 60 seconds so that the resin layer was in contact with the FR-4 substrate. The resin layer was then cured by heating in a hot air circulation drying oven at 100°C for 30 minutes, then at 180°C for 30 minutes. The release PET film was then peeled off to obtain a mounted substrate.
[0090] The resulting mounting substrate was cut with an ultrasonic cutter, and the cut surface was observed and measured using a field emission scanning electron microscope (FE-SEM) at a magnification of 100 to 1000 times to confirm the thickness of the resin layer from the substrate and the thickness from the top of each chip.
[0091] <Effect of suppressing occurrence of die marks> The surface of the sealing layer was visually observed, and the effect of suppressing occurrence of die marks was confirmed according to the following evaluation criteria: ◎: No die marks are visible (it is impossible to tell what is inside the sealing layer by looking at the surface of the sealing layer) ○: Die marks are faintly visible (it is possible to tell what is inside the sealing layer by looking at the surface of the sealing layer) ×: Die marks are clearly visible (the number of die marks can be seen by looking at the surface of the sealing layer) The evaluation results are shown in Table 2 below.
[0092] <Sealing Layer Penetration> The resulting mounting substrate was cut using an ultrasonic cutter, and the cut pieces were sealed with resin. The cut pieces were then polished using an ion milling machine so that the cut surfaces of the cut pieces were exposed. The polishing was performed so that the substrate cross section was roughly at the center of the chip. The exposed surfaces of the polished cut pieces were then observed and measured using an FE-SEM at magnifications of 100 to 1000 times, and the thickness of the sealing layer between the substrate and the chip (i.e., the amount of the dry film resin layer that penetrated between the substrate and the chip when forming the sealing layer) was measured. Good: The thickness of the sealing layer between the substrate and each chip was less than 40 μm. Bad: The thickness of the sealing layer between the substrate and each chip was 40 μm or more. The evaluation results are shown in Table 2 below.
[0093] [Example 2] A mounting substrate was produced in the same manner as in Example 1, except that Dry Film 1 in Example 1 was changed to Dry Film 2, and the evaluation of die mark suppression and penetration into the sealing layer was carried out in the same manner as above. The evaluation results are shown in Table 2 below.
[0094] [Example 3] In Example 1, the organic substrate was changed to a 0.4 mm thick organic substrate on which three types of chips with thicknesses of 165 μm, 220 μm, and 200 μm were mounted at 0.5 mm intervals with a gap of 10 to 15 μm from the substrate, and dry film 1 was changed to dry film 3. Except for this, a mounting substrate was produced in the same manner as in Example 1, and an evaluation of die mark suppression and penetration of the sealing layer was performed in the same manner as above. The evaluation results are shown in Table 2 below.
[0095] Comparative Example 1 A mounting substrate was prepared in the same manner as in Example 1, except that Dry Film 1 in Example 1 was changed to Dry Film 4, and the evaluation of die mark suppression and penetration of the sealing layer was performed in the same manner as above. The evaluation results are shown in Table 2 below.
[0096] Comparative Example 2 A mounting substrate was prepared in the same manner as in Example 1, except that Dry Film 1 in Example 1 was changed to Dry Film 5, and the evaluation of die mark suppression and penetration into the sealing layer was performed in the same manner as above. The evaluation results are shown in Table 2 below.
[0097]
[0098] As is clear from Table 2, T:t n It can be seen that in the mounting substrates (Examples 1 to 3) in which a sealing layer is formed using a curable resin composition containing a T:t ratio of 10:1.0 to 10:5.0 and a colorant in a proportion of 0.60 to 4.0 mass %, the occurrence of die marks can be suppressed even when a plurality of semiconductor chips of different sizes are mounted. n Even when the sealing layer is formed so that the ratio of T to t is 10:1.0 to 10:5.0, it is found that the occurrence of die marks cannot be suppressed unless the sealing layer is formed using a curable resin composition that does not contain a colorant in a proportion of 0.60 to 4.0 mass% (Comparative Example 1). n It can be seen that even when the thickness is such that the ratio exceeds 10:5.0, the occurrence of die marks cannot be suppressed (Comparative Example 2).
[0099] REFERENCE SIGNS LIST 1 Mounting substrate 10 Substrate 20A, 20B Unit of multiple semiconductor chips 201, 202, . . . 216 Semiconductor chip 30 Sealing layer 40 Dry film 401 First film 402 Resin layer 403 Second film
Claims
1. A mounting substrate comprising: a substrate; a plurality of semiconductor chips mounted on at least one surface of the substrate; and a sealing layer covering the substrate surface on which the plurality of semiconductor chips are mounted; wherein, in a thickness direction of the mounting substrate, a thickness of the sealing layer is T, and a distance from an upper surface of each semiconductor chip mounted on the substrate to a surface of the sealing layer is t n , then T:t n 10:1.0 to 10:5.0, and the sealing layer is made of a cured product of a curable resin composition containing a colorant in a ratio of 0.60 to 4.0 mass %.
2. t above n The mounting board according to claim 1 , wherein the thickness is 50 μm or more.
3. The mounting board according to claim 1, wherein T is 100 to 500 μm.
4. The mounting board according to claim 1, wherein the curable resin composition further contains a thermosetting resin.
5. The mounting board according to claim 1, wherein said coloring agent includes carbon black and titanium black.
6. The mounting board according to claim 1, wherein the curable resin composition further contains a thermoplastic resin having a glass transition point of 20° C. or lower and a weight average molecular weight of 30,000 or more.
7. The mounting board according to claim 5, wherein the colorant contains carbon black and titanium black in a ratio of 1:1.1 to 1:7 by mass.
8. The mounting board according to claim 1, wherein three to six of the semiconductor chips form one unit, and the distance between adjacent units is 1 mm or less.
Citation Information
Patent Citations
Resin composition for encapsulation and semiconductor device
JP2018162351A
Cited By
Resin sheet for sealing hollow electronic components and hollow electronic components
JP7764986B1