Surface-treated steel sheet
The surface-treated steel sheet with a zinc-nickel plating layer and a specific coating composition improves corrosion resistance and workability, addressing the limitations of existing sheets in fuel tank applications by maintaining low crack ratios and enhanced protection against fuels.
Patent Information
- Application Number
- PCT/JP2024/013085
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
Existing surface-treated steel sheets used for fuel tanks lack sufficient corrosion resistance after forming, despite having formability and corrosion resistance requirements.
A surface-treated steel sheet with a zinc-nickel plating layer and a coating film containing epoxy resin, isocyanate resin, silica particles, and polyethylene wax, where the coating film has a thickness of 0.5 to 2.0 μm and a Si-enriched region at the interface, allowing for improved corrosion resistance by maintaining a crack ratio of 80% or less after tensile elongation.
The solution significantly enhances corrosion resistance and workability of the steel sheet, ensuring effective protection against fuels like gasoline and maintaining structural integrity post-processing.
Smart Images

Figure JP2024013085_03102024_PF_FP_ABST
Abstract
Description
Surface-treated steel sheet
[0001] The present invention relates to a surface-treated steel sheet.
[0002] Various types of plated steel sheets are used as materials for manufacturing motorcycle fuel tanks. When manufacturing a fuel tank, the plated steel sheet material must be processed into the desired shape. Furthermore, the surface of the plated steel sheet that is exposed to fuels such as gasoline must be corrosion-resistant to prevent corrosion by the fuel. Therefore, plated steel sheets used as fuel tank materials must be both formable and corrosion-resistant.
[0003] In order to achieve both formability and corrosion resistance, for example, Patent Document 1 listed below discloses an organic composite plated steel sheet in which a chromate film and a film made of a paint composition are formed on the surface of a zinc, aluminum, or zinc-based alloy plated steel sheet.
[0004] Special Publication No. 4-28539
[0005] Here, the present inventors have further studied the organic composite plated steel sheet disclosed in Patent Document 1 and have found that there is room for further improvement in corrosion resistance after forming.
[0006] Therefore, the present invention has been made in consideration of the above problems, and an object of the present invention is to provide a surface-treated steel sheet that can further improve corrosion resistance after forming.
[0007] In order to solve the above problems, the present inventors conducted extensive research and came to the conclusion that even when stress is applied to a surface-treated steel sheet due to processing, if a coating film provided above a plating layer can appropriately deform in response to the stress, it is possible to further improve corrosion resistance after processing. The gist of the present invention, which was completed based on this finding, is as follows.
[0008] (1) A surface-treated steel sheet comprising a zinc- and nickel-containing plating layer located on at least one surface of the steel sheet, and a coating film located on the plating layer and containing at least an epoxy resin and an isocyanate resin, wherein, when a cross section cut in the thickness direction after applying a 10% tensile elongation is observed, the ratio of the total length of cracks generated in the coating film to the total length of cracks generated in the plating layer within a 60 μm long region in a direction perpendicular to the thickness direction is 80% or less. (2) A surface-treated steel sheet according to (1), wherein a Si-enriched region is present at the interface between the plating layer and the coating film, and the plating layer has a concentration gradient in which the Zn concentration at the interface on the coating film side is higher than the Zn concentration at the interface on the plating layer side. (3) The surface-treated steel sheet according to (1) or (2), wherein the coating film has a thickness of 0.5 to 2.0 μm. (4) The surface-treated steel sheet according to (1) or (2), wherein the epoxy resin is a bisphenol A-type epoxy resin having a number-average molecular weight of 300 to 100,000. (5) The surface-treated steel sheet according to (4), wherein the coating film further contains silica particles. (6) The surface-treated steel sheet according to (5), wherein the coating film further contains polyethylene wax, the content of the epoxy resin is 30.0 mass% or more relative to the coating film solid content, the content of the isocyanate resin is 0.1 to 2.0 mass% relative to the epoxy resin, the content of the silica particles is 5.0 to 50.0 mass% relative to the coating film solid content, and the content of the polyethylene wax is 0.1 to 10.0 mass% relative to the coating film solid content, and the coating film contains the epoxy resin, the isocyanate resin, the silica particles, and the polyethylene wax in a total amount of 100 mass% or less. (7) The surface-treated steel sheet according to (5) or (6), wherein the silica particles are at least one of fumed silica and colloidal silica, the fumed silica having an average particle size of 5 to 40 nm, and the colloidal silica having an average particle size of 5 to 200 nm. (8) The surface-treated steel sheet according to (1) or (2), further comprising a chemical conversion coating between the plating layer and the coating film, the chemical conversion coating having a thickness of 10 to 1000 nm.(9) The surface-treated steel sheet according to (1) or (2), which is used as a material for a fuel tank.
[0009] As described above, according to the present invention, it is possible to further improve the corrosion resistance after forming.
[0010] Fig. 1 is an explanatory diagram schematically showing one example of the structure of a surface-treated steel sheet according to an embodiment of the present invention; Fig. 2 is an explanatory diagram schematically showing another example of the structure of a surface-treated steel sheet according to the same embodiment; Fig. 3 is an explanatory diagram for explaining a Si-enriched region in a surface-treated steel sheet according to the same embodiment; Fig. 4 is an explanatory diagram for explaining cracks that occur after tensile elongation is imparted to the surface-treated steel sheet according to the same embodiment; Fig. 5 is a flow chart showing one example of the flow of a manufacturing method of a surface-treated steel sheet according to the same embodiment;
[0011] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. In this specification and drawings, components having substantially the same functional configurations are designated by the same reference numerals, and redundant explanations will be omitted.
[0012] (Regarding Surface-Treated Steel Sheet) Hereinafter, a surface-treated steel sheet according to an embodiment of the present invention will be described in detail.
[0013] <Overall Configuration of Surface-Treated Steel Sheet> First, the overall configuration of the surface-treated steel sheet according to this embodiment will be described with reference to Figures 1A and 1B. Figure 1A is an explanatory view schematically showing one example of the structure of the surface-treated steel sheet according to this embodiment, and Figure 1B is an explanatory view schematically showing another example of the structure of the surface-treated steel sheet according to this embodiment.
[0014] As shown schematically in Fig. 1A, the surface-treated steel sheet 1 according to this embodiment has a steel sheet 10, a plating layer 20, and a coating film 30. As shown schematically in Fig. 1B, the surface-treated steel sheet 1 according to this embodiment may further have a chemical conversion coating 40 between the plating layer 20 and the coating film 30. The surface-treated steel sheet 1 having the configuration shown in Fig. 1A or 1B can be suitably used as a material for fuel tanks of various automobiles (particularly motorcycles).
[0015] 1A and 1B illustrate a case where the plating layer 20, the coating film 30, and the chemical conversion coating 40 are provided on one surface of the steel sheet 10, but these plating layer 20, the coating film 30, and the chemical conversion coating 40 may be provided on both surfaces of the steel sheet 10.
[0016] [Regarding the Steel Plate 10] The steel plate 10 is the base material of the surface-treated steel plate 1 according to this embodiment, and various steel plates can be used depending on the strength (e.g., tensile strength) required of the surface-treated steel plate 1. Examples of such steel plates include ordinary steel, low-carbon steel, and high-strength steel.
[0017] However, when manufacturing a fuel tank, which is one of the important applications of the surface-treated steel sheet 1 according to this embodiment, a high degree of workability is required for the steel sheet used as the raw material. Therefore, it is preferable to use IF steel, which has excellent workability, as the steel sheet 10 according to this embodiment, and furthermore, it is more preferable to use a steel sheet containing several ppm or more of boron (B) in order to ensure airtightness after welding, secondary workability, etc.
[0018] The thickness of the steel plate 10 may also be set appropriately depending on the strength required of the surface-treated steel plate 1 and the allowable mass of the article manufactured by processing the surface-treated steel plate 1, etc.
[0019] [Regarding the plating layer 20] The plating layer 20 in the surface-treated steel sheet 1 is a layer provided to ensure the corrosion resistance of the base material, the steel sheet 10. The plating layer 20 according to this embodiment is located on at least one surface of the steel sheet 10, and is a plating layer containing zinc (Zn) and nickel (Ni).
[0020] By providing the plating layer 20 containing zinc and nickel, the plating layer 20 exhibits excellent resistance weldability, workability, and corrosion resistance (particularly, gasoline resistance). In the plating layer 20, the Ni content is preferably within a range of 5 to 15 mass %, with the remainder being Zn and impurities.
[0021] By setting the Ni content to 5% by mass or more, it is possible to further improve corrosion resistance without causing a decrease in resistance weldability and workability. The Ni content is more preferably 8% by mass or more. On the other hand, by setting the Ni content to 15% by mass or less, it is possible to further suppress the occurrence of large cracks in the plating layer 20 and further ensure the adhesion of the plating layer 20. The Ni content is more preferably 13% by mass or less.
[0022] The coating weight of the plating layer 20 is 2 to 50 g / m 2 It is preferable that the coating weight of the plating layer 20 is within the range of 2 g / m 2 By setting the coating weight at or above, it becomes possible to fully exhibit the various properties of the plating layer 20, such as resistance weldability, workability, and corrosion resistance. The coating weight of the plating layer 20 is more preferably 10 g / m 2 On the other hand, when the coating weight of the plating layer 20 is 50 g / m 2 By setting the coating weight of the plating layer 20 to 40 g / m or less, it is possible to more favorably achieve both resistance weldability and workability, and corrosion resistance. 2 is
[0023] The coating mass of the plating layer 20 can be calculated from the difference in mass before and after physical or chemical removal of a known area of the plating layer 20 from the steel sheet 10. The method for removing the plating layer 20 from the steel sheet 10 is not particularly limited, but examples of physical methods include blasting, and examples of chemical methods include acid dissolution treatment. Alternatively, fluorescent X-ray analysis can be performed to calculate the coating mass of the plating layer from the measured intensity of zinc, the main component of the plating layer 20, using a calibration curve prepared from known zinc-nickel standard samples. The Ni content of the plating layer 20 can be determined by measuring the plating layer 20 removed from the steel sheet 10 as described above using an X-ray fluorescent analyzer.
[0024] Here, when the plating layer 20 according to this embodiment is measured by radio frequency glow discharge optical emission spectrometry (RF-Glow Discharge Optical Emission Spectrometry: RF-GD-OES), the plating layer 20 has a concentration gradient in which the Zn concentration increases toward the coating film 30 in the Zn depth profile obtained by the measurement. This state is achieved by a specific manufacturing method described below.
[0025] Zn, which is an element with a lower potential than Fe, is present in large amounts on the coating film 30 side of the plating layer 20, which makes it easier for the sacrificial corrosion protection effect of Zn to function, contributing to further improvement of corrosion resistance.
[0026] The concentration gradient of Zn in the plating layer 20 as described above can be confirmed as follows. That is, a depth profile is obtained from the surface side of the plating layer 20 by radio frequency glow discharge optical emission spectroscopy (RF-GD-OES). Then, within the thickness of the plating layer 20 calculated from the profile corresponding to the plating layer 20, the maximum intensity is calculated at a position located a thickness corresponding to ¼ of the layer thickness from the interface on the coating film 30 side toward the steel sheet 10 side, and the maximum intensity is calculated at a position located a thickness corresponding to ¼ of the total thickness from the interface on the steel sheet 10 side toward the coating film 30 side. In this case, if the Zn intensity on the coating film 30 side is higher than the Zn intensity on the steel sheet 10 side, it is defined as having a concentration gradient such that the Zn concentration is higher.
[0027] In the depth profile of radio frequency glow discharge optical emission spectroscopy (RF-GD-OES), in the depth profile of nickel, which is an element derived from the plating layer 20, the two positions where the nickel peak is reduced by half (the half-reduction position on the coating film 30 side and the half-reduction position on the steel sheet 10 side) can be defined as the interface of the plating layer 20 on the coating film 30 side and the interface of the plating layer 20 on the steel sheet 10 side, respectively.
[0028] The RF-GD-OES measurement may be carried out using a glow discharge optical emission surface analyzer (for example, a Marcus-type high-frequency glow discharge optical emission surface analyzer GD-Profiler 2 manufactured by Horiba Jobin Yvon Co., Ltd.) under conditions of a gas replacement time of 30 seconds, a pre-sputtering time of 30 seconds, a pressure of 600 Pa, and an output of 35 W, until the intensity of the spectrum of iron derived from the underlying steel is detected.
[0029] Here, in the plating layer 20 according to this embodiment, the maximum Zn intensity at 1 / 4 of the layer thickness on the coating film 30 side of the plating layer 20 is preferably 1.01 to 1.50 times the maximum Zn intensity at 1 / 4 of the layer thickness on the steel sheet 10 side. When the maximum Zn intensity ratio is within the above range, it is possible to achieve both adequate workability due to the Zn-rich surface layer of the plating layer 20 and good corrosion resistance due to Ni. The maximum Zn intensity ratio is more preferably 1.02 or more, and even more preferably 1.03 or more. Furthermore, the maximum Zn intensity ratio is more preferably 1.40 or less, and even more preferably 1.30 or less.
[0030] When identifying the state of the plating layer 20 from a surface-treated steel sheet that has already been processed into various parts such as a fuel tank, a test piece can be cut out from a portion of the part of interest that has not been subjected to joining processes such as welding or processing processes such as drawing or bending, and used as the object of analysis. In this case, the size of the test piece cut out can be the size of the test piece when made into a flat plate, for example, about 50 x 50 mm. A portion of the obtained test piece can be used to perform the above-mentioned RF-GD-OES measurement.
[0031] [Regarding the coating film 30] The coating film 30 according to this embodiment is located on the plating layer 20 or the chemical conversion coating 40, and is a resin layer containing at least an epoxy resin and an isocyanate resin. Preferably, the coating film 30 further contains either silica particles or polyethylene wax, or both. By providing the coating film 30, the surface-treated steel sheet 1 according to this embodiment exhibits excellent corrosion resistance, processability, and electrodeposition coatability.
[0032] <Epoxy Resin> The epoxy resin contained in the coating film 30 according to this embodiment is a resin that functions as a binder resin. By containing an epoxy resin in the coating film 30, the water resistance and alkali resistance of the coating film are improved, and adhesion to other layer structures is also improved. In the coating film 30 according to this embodiment, it is preferable to use, for example, a bisphenol A-type epoxy resin as the epoxy resin.
[0033] The number average molecular weight of the epoxy resin contained in the coating film 30 according to this embodiment is preferably within the range of 300 to 100,000.
[0034] By setting the number average molecular weight of the epoxy resin to 300 or more, the resin can be sufficiently polymerized by a crosslinking reaction, thereby further improving the corrosion resistance of the coating film. The number average molecular weight of the epoxy resin is more preferably 1,000 or more, and even more preferably 2,000 or more. On the other hand, by setting the number average molecular weight of the epoxy resin to 100,000 or less, the resin can be sufficiently polymerized by a crosslinking reaction, thereby further improving the corrosion resistance of the coating film. The number average molecular weight of the epoxy resin is more preferably 20,000 or less, and even more preferably 10,000 or less.
[0035] Furthermore, among epoxy resins having a number-average molecular weight within the above range, it is even more preferable to use those having an epoxy equivalent in the range of 1000 to 3500. By setting the epoxy equivalent of the epoxy resin to 1000 or more, it is possible to more appropriately crosslink the epoxy resin and further improve the corrosion resistance of the coating film. The epoxy equivalent of the epoxy resin is more preferably 1500 or more, and even more preferably 2000 or more. On the other hand, by setting the epoxy equivalent of the epoxy resin to 3500 or less, it is possible to suppress excessive polymerization of the epoxy resin, thereby maintaining the processability of the coating film 30 and further improving the corrosion resistance of the coating film. The epoxy equivalent of the epoxy resin is more preferably 3000 or less, and even more preferably 2500 or less.
[0036] From the above viewpoints, it is more preferable to use a bisphenol A type epoxy resin having a number average molecular weight in the range of 300 to 100,000 and an epoxy equivalent in the range of 1,000 to 3,500 as the epoxy resin in the coating film 30 according to this embodiment.
[0037] <Isocyanate Resin> The isocyanate resin contained in the coating film 30 according to this embodiment is a resin that functions as a curing agent, and is able to appropriately cure the coating film 30 to exhibit excellent corrosion resistance, processability, and adhesion. Here, the isocyanate resin according to this embodiment refers to a resin having an isocyanate group or a low-molecular-weight compound having an isocyanate group, and examples of such isocyanate resins include polyisocyanate compounds and blocked polyisocyanate compounds.
[0038] Examples of the polyisocyanate compound include an aliphatic or alicyclic diisocyanate compound, an aromatic diisocyanate compound, and a triisocyanate compound.
[0039] Examples of aliphatic or alicyclic diisocyanate compounds include hexamethylene diisocyanate, isophorone diisocyanate, hydrogenated diphenylmethane diisocyanate, etc. Examples of aromatic diisocyanate compounds include tolylene diisocyanate, diphenylmethane-4,4'-diisocyanate, etc. Examples of triisocyanate compounds include adducts of 1 mole of trimethylolpropane and 3 moles of the above diisocyanates, and trimers of diisocyanates such as hexamethylene diisocyanate and tolylene diisocyanate.
[0040] The blocked polyisocyanate compound is a polyisocyanate compound such as those exemplified above that is blocked with a blocking agent. Preferably, the blocking agent is one that, when added to an isocyanate group, produces an adduct that is stable at room temperature and dissociates to regenerate free isocyanate groups when the coating film is baked.
[0041] Examples of such blocking agents include lactam-based blocking agents, oxime-based blocking agents, alcohol-based blocking agents, phenol-based blocking agents, and ester-based blocking agents.
[0042] Here, examples of lactam-based blocking agents include ε-caprolactam and γ-butyrolactam. Examples of oxime-based blocking agents include methyl ethyl ketoxime and cyclohexanone oxime. Examples of alcohol-based blocking agents include methanol, ethanol, and isobutyl alcohol. Examples of phenol-based blocking agents include phenol, p-tert-butylphenol, and cresol. Examples of ester-based blocking agents include ethyl acetoacetate and methyl acetoacetate. Among the above-mentioned blocking agents, methyl ethyl ketoxime and ethyl acetoacetate are particularly preferred, from the viewpoints that they dissociate particularly at low temperatures and are stable during storage of the coating material for forming a coating film.
[0043] In the coating film 30 according to this embodiment, the above-mentioned polyisocyanate compounds and blocked polyisocyanate compounds can be used alone or in combination of two or more. The compounds exemplified above are merely examples of isocyanate resins, and isocyanate resins other than those mentioned above can also be used.
[0044] <Silica Particles> The silica particles that are preferably contained in the coating film 30 according to this embodiment are components that are contained to prevent components in the coating film 30 from eluting out of the coating film, while further improving the corrosion resistance of the coating film 30. Examples of such silica particles include fumed silica and colloidal silica. At least one of these silica particles is used in the coating film 30 according to this embodiment.
[0045] Here, the average particle size of the fumed silica is preferably within the range of 5 to 40 nm. By setting the average particle size of the fumed silica to 5 nm or more, it is possible to further improve the corrosion resistance and adhesion of the coating film 30. The average particle size of the fumed silica is more preferably 7 nm or more. On the other hand, by setting the average particle size of the fumed silica to 40 nm or less, it is possible to further improve the corrosion resistance while maintaining the smoothness of the coating film 30. The average particle size of the fumed silica is more preferably 16 nm or less.
[0046] Furthermore, the average particle size of the colloidal silica is preferably within the range of 5 to 200 nm. By setting the average particle size of the colloidal silica to 5 nm or more, it is possible to further improve the corrosion resistance and adhesion of the coating film 40. The average particle size of the colloidal silica is more preferably 9 nm or more, and even more preferably 12 nm or more. On the other hand, by setting the average particle size of the colloidal silica to 200 nm or less, it is possible to further improve the corrosion resistance while maintaining the smoothness of the coating film 30. The average particle size of the colloidal silica is more preferably 60 nm or less, and even more preferably 22 nm or less.
[0047] <Polyethylene Wax> The polyethylene wax that is preferably contained in the coating film 30 according to this embodiment functions as a lubricant and further improves the workability of the surface-treated steel sheet 1 according to this embodiment. In particular, it is preferable to use, as this polyethylene wax, a polyethylene wax having a density of 0.94 or more, a molecular weight in the range of 1,000 to 10,000, and an acid value of 15 KOHmg / g or less. By using a polyethylene wax having the above-mentioned density, molecular weight, and acid value, it is possible to further improve the workability of the surface-treated steel sheet 1.
[0048] Furthermore, in addition to the polyethylene wax, the coating film 30 according to this embodiment may contain various lubricants such as polyolefin-based lubricants, carboxylic acid ester-based lubricants, metal carboxylic acid salts, and polyalkylene glycol-based lubricants, as well as various lubricant powders such as molybdenum disulfide, silicone compounds, and fluorine compounds.
[0049] <Contents of the Above Components> In the coating film 30 according to this embodiment, the contents of the epoxy resin, isocyanate resin, silica particles, and polyethylene wax preferably satisfy the following conditions: the epoxy resin content is 30.0 mass% or more relative to the coating solid content (i.e., relative to the total mass of the coating film 30), the isocyanate resin content is 0.10 to 2.00 in mass ratio relative to the epoxy resin, the silica particle content is 5.0 to 50.0 mass% relative to the coating solid content (i.e., relative to the total mass of the coating film 30), and the polyethylene wax content is 0.1 to 10.0 mass% relative to the coating solid content (i.e., relative to the total mass of the coating film 30), and the epoxy resin, isocyanate resin, silica particles, and polyethylene wax are preferably contained in a total amount of 100 mass% or less.
[0050] By setting the epoxy resin content to 30.0% by mass or more relative to the total mass of the coating film solids (i.e., coating film 30), it is possible to suppress embrittlement of the coating film 30 and further improve the processing adhesion of the coating film 30. The epoxy resin content is more preferably 45.0% by mass or more, and even more preferably 50.0% by mass or more, relative to the coating film solids.
[0051] By setting the mass ratio of the isocyanate resin to the epoxy resin to be 0.10 or more, the epoxy resin and the isocyanate resin can be crosslinked in a favorable state, thereby realizing a coating film with excellent corrosion resistance. The mass ratio of the isocyanate resin to the epoxy resin is more preferably 0.15 or more, and even more preferably 0.20 or more. On the other hand, by setting the mass ratio of the isocyanate resin to the epoxy resin to be 2.00 or less, the water resistance and alkali resistance of the coating film 30 can be maintained while further improving the adhesion of the coating film 30. The mass ratio of the isocyanate resin to the epoxy resin is more preferably 0.90 or less, and even more preferably 0.50 or less.
[0052] By setting the content of silica particles to 5.0 mass% or more relative to the total mass of the coating solids (i.e., the coating 30), it is possible to further improve the corrosion resistance of the coating 40. The content of silica particles is more preferably 18.0 mass% or more, and even more preferably 23.0 mass% or more, relative to the coating solids. On the other hand, by setting the content of silica particles to 50.0 mass% or less, relative to the total mass of the coating solids, it is possible to prevent a decrease in the processing adhesion of the coating 30. The content of silica particles is more preferably 38.0 mass% or less, and even more preferably 33.0 mass% or less, relative to the coating solids.
[0053] By setting the polyethylene wax content to 0.1% by mass or more relative to the total mass of the coating solids (i.e., the coating 30), it is possible to reduce the frictional resistance of the surface of the coating 30 and prevent peeling of the coating during processing. The polyethylene wax content is more preferably 1.0% by mass or more, and even more preferably 1.5% by mass or more, relative to the coating solids. On the other hand, by setting the polyethylene wax content to 10.0% by mass or less relative to the total mass of the coating solids, it is possible to prevent the occurrence of shrinkage unevenness of the polyethylene wax and achieve a coating 30 with excellent appearance. The polyethylene wax content is more preferably 3.0% by mass or less, and even more preferably 2.5% by mass or less, relative to the coating solids.
[0054] <<Regarding Other Components>> In addition to the components described above, the coating film 30 according to this embodiment may further contain a resol-type phenolic resin. By further containing a resol-type phenolic resin in the coating film 30, the coating film formation reaction can be promoted at lower temperatures (for example, a maximum temperature of approximately 100 to 130°C). In this case, the content of the resol-type phenolic resin relative to the content of the isocyanate resin is preferably, for example, within a range of 0.1 to 10.0 in terms of mass ratio. This makes it possible to promote the coating film formation reaction at lower temperatures while suppressing a decrease in the alkali resistance of the coating film 30.
[0055] Furthermore, the coating film 30 according to this embodiment may further contain, in addition to the components described above, an anti-rust pigment, an extender pigment, a coloring pigment, an anti-rust agent, a dispersion stabilizer, and the like.
[0056] <<About Thickness>> In the coating film 30 according to this embodiment, the thickness of the coating film 30 (d1 in FIGS. 1A and 1B) is within the range of 0.5 to 2.0 μm. If the thickness d1 of the coating film 30 is less than 0.5 μm, the coating film 30 is too thin, and the surface-treated steel sheet 1 cannot exhibit sufficient corrosion resistance. By setting the thickness d1 of the coating film 30 to 0.5 μm or more, the surface-treated steel sheet 1 can exhibit excellent corrosion resistance even when exposed to various fuels including gasoline. The thickness d1 of the coating film 30 is preferably 0.6 μm or more, and more preferably 0.7 μm or more.
[0057] On the other hand, if the thickness d1 of the coating film 30 exceeds 2.0 μm, this is not preferred because it may deteriorate the spot weldability and appearance of the surface-treated steel sheet 1. By setting the thickness d1 of the coating film 30 to 2.0 μm or less, it is possible to suppress deterioration in spot weldability and appearance while achieving excellent corrosion resistance. The thickness d1 of the coating film 30 is preferably 1.5 μm or less.
[0058] Here, the thickness d1 of the coating film 30 can be measured by direct observation of the cross section. Specifically, the surface-treated steel sheet of interest is embedded in a room-temperature drying epoxy resin so that the cross section in the thickness direction can be observed, and the embedded surface is mechanically polished and further polished to a mirror finish, and then observed with a scanning electron microscope (SEM). The thickness can be measured at any number of positions (e.g., 10 positions), and the average value of the obtained thicknesses can be used as the thickness of the coating film 30. In this case, the coating film 30 may be identified in combination with elemental mapping using energy dispersive X-ray spectrometry (EDS) or an electron probe microanalyzer (EPMA).
[0059] Furthermore, the film thickness can be converted into the thickness of the coating film 30 per unit sputtering time by measuring the depth profile from the surface side of the surface-treated steel sheet to the steel sheet side using radio frequency glow discharge optical emission spectroscopy (RF-GD-OES) and comparing the sputtering time corresponding to the depth profile of the coating film 30 with the thickness of the coating film 30 observed by SEM from the cross section described above.
[0060] Here, when identifying the details of the coating film 30 from a surface-treated steel sheet that has already been processed into various parts such as a fuel tank, a test piece can be cut out from a portion of the part of interest that has not been subjected to joining processes such as welding or processing processes such as drawing or bending, and used as the object of analysis. In this case, the size of the test piece cut out can be the size when the test piece is made into a flat plate, for example, about 50 x 50 mm. Various measurements can then be performed using the obtained test piece. Various measurements can then be performed using the obtained test piece.
[0061] For example, when determining the content of the above-mentioned components in a portion of a test piece corresponding to the coating film 30, the portion corresponding to the coating film 30 can be analyzed by Fourier transform infrared spectroscopy (FT-IR) and the components can be determined based on whether or not peaks derived from epoxy groups or isocyanate groups are detected in the resulting infrared absorption spectrum. If peaks derived from epoxy groups are detected in the resulting infrared absorption spectrum, it can be determined that the coating film 30 of interest contains an epoxy resin. Furthermore, if peaks derived from isocyanate groups are detected in the resulting infrared absorption spectrum, it can be determined that the coating film 30 of interest contains an isocyanate resin.
[0062] The contents of the epoxy resin and isocyanate resin can be determined by preparing an epoxy resin / isocyanate resin mixed coating film in advance, the mixing ratio of which is known, and creating a calibration curve of the peak intensity of the peak derived from the epoxy group and the peak intensity of the peak derived from the isocyanate group for the mixed coating film by FT-IR.Then, in the analysis by FT-IR obtained as described above, the contents of the epoxy resin and isocyanate resin can be specified from the peak intensity of each peak obtained.
[0063] The number average molecular weight of the epoxy resin can be determined as follows: A sample is taken from the portion of the test piece corresponding to the coating film 30, and the molecular structure of the resin is analyzed by field desorption mass spectrometry (FD-MS) to determine its molecular weight distribution.
[0064] The presence or absence of polyethylene wax can be determined by immersing a test piece in a heated solvent (more specifically, 2-butanone heated to approximately 80°C) to dissolve and separate the polyethylene wax in the solvent, analyzing the resulting extract by FT-IR, and determining whether or not a peak derived from a methylene group is detected in the resulting infrared absorption spectrum. If a peak derived from a methylene group is detected in the resulting infrared absorption spectrum, it can be determined that the coating film 30 of interest contains polyethylene wax. The content ratio of polyethylene wax can be determined from the difference in mass between before and after extraction of the polyethylene wax as described above.
[0065] Furthermore, the presence or absence of silica particles can be identified, for example, by confirming the presence of elements Si and O by elemental analysis such as X-ray fluorescence analysis for a portion of the test piece corresponding to the coating film 30, and then analyzing the portion corresponding to the coating film 30 by FT-IR, based on whether or not a peak derived from an Si—O bond is detected in the resulting infrared absorption spectrum. If the presence of elements Si and O is confirmed by elemental analysis and a peak derived from an Si—O bond is detected in the infrared absorption spectrum, it can be determined that the coating film 30 of interest contains silica particles.
[0066] The average particle size of the silica particles can be calculated by cutting a cross section of the coating film using a focused ion beam (FIB) or an ultramicrotome and observing the silica particles using a transmission electron microscope (TEM). The content of the silica particles can be calculated by converting the amount of Si obtained by analyzing a region of, for example, 30 mmφ of the coating film 30 using fluorescent X-ray analysis into the content of silica particles.
[0067] [Regarding the Si-enriched Region] As will be explained again below, the surface-treated steel sheet 1 according to this embodiment is manufactured by forming a plating layer on the surface of a steel sheet, and then applying a paint to form a coating film on the plating layer (in the case of the configuration shown in FIG. 1A ), or by forming a plating layer on the surface of a steel sheet, and then forming a chemical conversion coating on the plating layer, and then applying a paint to form a coating film on the chemical conversion coating (in the case of the configuration shown in FIG. 1B ). Here, when the paint is solidified to form a coating film, the coated steel sheet is subjected to a predetermined heat treatment.
[0068] When the surface-treated steel sheet 1 according to this embodiment has a chemical conversion coating layer 40 as described in detail below, the coating of the above-described paint often etches the underlying chemical conversion coating, causing components in the chemical conversion coating to diffuse into the paint. Furthermore, during such heat treatment, components of the plating layer, components of the paint, etc., diffuse into each other, regardless of whether the chemical conversion coating layer 40 is present or not.
[0069] As explained above, the plating layer 20 according to this embodiment has a concentration gradient in which the Zn concentration increases toward the coating film 30. While the detailed mechanisms of the etching and heat treatment described above are unknown, the uneven distribution of Zn causes Si, one of the components of the coating film 30, to concentrate at the interface between the coating film 30 and the plating layer 20 (or, depending on the degree of etching or heat treatment, between the coating film 30 and the chemical conversion coating 30), forming a Si-enriched region 50 as shown schematically in Fig. 2. Note that Fig. 2 illustrates an example in which the Si-enriched region 50 is formed between the coating film 30 and the plating layer 20. Furthermore, in FIG. 2 , for convenience of drawing, the Si-enriched region 50 is illustrated as if it were a region separate from the coating film 30. However, the Si-enriched region 50 is a region that exists as part of the coating film 30, and as shown in FIG. 2 by the dashed line indicating the boundary of the Si-enriched region 50 on the side opposite to the plating layer 20, there is no clear boundary between the Si-enriched region 50 and the coating film layer 30.
[0070] Due to the presence of a large amount of Si, such Si-enriched regions 50 are able to follow the applied tensile elongation to a certain extent when tensile elongation is imparted to the surface-treated steel sheet 1 by a forming process. Furthermore, the presence of such Si-enriched regions 50 also improves adhesion with the underlying chemical conversion treatment layer 40 or plating layer 20. As a result, the Si-enriched regions 50 act advantageously in improving adhesion between the coating film 30 and the plating layer 20 or chemical conversion treatment film 40.
[0071] The presence of the Si-enriched region 50 can be confirmed as follows. That is, a range from the surface of the coating film 40 to approximately the interface between the plating layer 20 and the steel sheet 10 is measured by radio frequency glow discharge optical emission spectroscopy to obtain a Si depth profile. Then, the presence of the Si-enriched region 50 can be confirmed by the presence of a Si peak on the plating layer 20 side of the coating film 30 in the obtained Si depth profile.
[0072] The above-mentioned peak refers to a portion near the interface of the coating film 30 on the plating layer 20 side where the Si intensity is 1.1 times or more the Si intensity at the center in the thickness direction of the coating film 30. The Si peak is assumed to be present within ⅓ of the thickness of the coating film 30 from the interface on the plating layer 20 side toward the center in the thickness direction of the coating film 30.
[0073] Here, when identifying the Si-enriched region 50 from a surface-treated steel sheet that has already been processed into various parts such as a fuel tank, a test piece may be cut out from a portion of the part of interest that has not been subjected to joining processes such as welding or processing processes such as drawing or bending, and used as the object of analysis. In this case, the size of the test piece to be cut out may be the size of the test piece when made into a flat plate, for example, about 50 × 50 mm. Then, the above-mentioned measurements may be carried out using the obtained test piece.
[0074] [Regarding cracking of coating film when tensile elongation is applied] Cracking of the coating film when tensile elongation is applied to the surface-treated steel sheet 1 according to this embodiment will be described with reference to Fig. 3. Fig. 3 is an explanatory diagram for explaining cracking that occurs after tensile elongation is applied to the surface-treated steel sheet according to this embodiment.
[0075] When the surface-treated steel sheet 1 according to this embodiment is subjected to a 10% tensile elongation and a cross section cut in the thickness direction is observed, the ratio of the total length of cracks generated in the coating film 30 to the total length of cracks generated in the plating layer 20 within a region 60 μm long in a direction perpendicular to the thickness direction is 80% or less. A specific description will be given below with reference to Fig. 3. Note that Fig. 3 illustrates an example in which the surface-treated steel sheet 1 has the plating layer 20, the chemical conversion coating 40, and the coating film 30.
[0076] After imparting a 10% tensile elongation to the surface-treated steel sheet 1, a cross section cut in the thickness direction is observed under a microscope at a magnification such that a region 60 μm in length can be observed in the direction perpendicular to the thickness direction (the tensile direction in FIG. 3 ).
[0077] The 10% tensile elongation imparted to the surface-treated steel sheet 1 causes fractured portions to be present in the plating layer 20, the chemical conversion coating 40, and the paint film 30. In this case, the length of each fractured portion along the direction perpendicular to the thickness direction is defined as the crack length.
[0078] In the example shown in Figure 3, there are three types of cracks in the plating layer 20: a crack with a length La, a crack with a length Lb, and a crack with a length Lc. Therefore, the total length of the cracks that have occurred in the plating layer 20 within a 60 µm long region is (La + Lb + Lc). On the other hand, there is a crack with a length L1 in the coating film 30. Therefore, the total length of the cracks that have occurred in the coating film 40 within a 60 µm long region is L1.
[0079] Therefore, in the example shown in Figure 3, the ratio of the total length of the cracks that have occurred in the coating film 30 to the total length of the cracks that have occurred in the plating layer 20 is {L1 / (La + Lb + Lc)} × 100 [unit: %].
[0080] The above-described observation is performed on multiple visual fields (e.g., 10 visual fields), and the above-described ratio is calculated for each visual field. The ratios obtained from the respective visual fields are then averaged over the number of visual fields observed, and this is treated as the ratio of the total length of cracks occurring in the coating film 30 to the total length of cracks occurring in the plating layer 20.
[0081] If this ratio exceeds 80%, the coating film 30 will not be able to follow the tensile elongation, resulting in excessive cracking of the coating film 30 and making it impossible to exhibit sufficient corrosion resistance. If this ratio is 80% or less, the surface-treated steel sheet 1 will exhibit excellent corrosion resistance even after forming. This ratio is preferably 60% or less, more preferably 50% or less, and even more preferably 40% or less. On the other hand, the smaller this ratio is, the better, and the lower limit thereof may be 0%.
[0082] [Regarding the chemical conversion coating 40] The chemical conversion coating 40 according to this embodiment is provided on the plating layer 20 as needed, and is a layer provided to improve the adhesion between the plating layer 20 and the coating film 30 and to improve the corrosion resistance of the surface-treated steel sheet 1.
[0083] Here, the chemical conversion coating 40 according to this embodiment may be a so-called chromate coating containing the element Cr, or may be a so-called chromate-free coating not containing the element Cr.
[0084] When a chromate film is provided as the chemical conversion film 40, the chromate film may be formed according to a conventional treatment method such as electrolytic chromate treatment, immersion chromate treatment, paint-on chromate treatment, or reactive chromate treatment.
[0085] In the case of immersion type chromate treatment, paint type chromate treatment, and reactive type chromate treatment, Cr 6+ , Cr 3+ The main component is SiO 2 and TiO 2 It is possible to use a chromate treatment solution containing inorganic colloids such as Cr, acids such as phosphoric acid and molybdic acid, or their salts, fluorides, or water-soluble or emulsion-type organic resins. 6+ , Cr 3+ The chromate treatment solution contains sulfuric acid and halogen ions as the main component, and in addition to these components, further contains SiO 2 and TiO 2 It is possible to use a chromate treatment solution containing inorganic colloids such as those mentioned above, or metal ions such as Co and Zn.
[0086] The chromate film formed using the above-mentioned chromate treatment solution is preferably a sparingly soluble chromate film having a water-soluble content of 5% or less. By forming a sparingly soluble chromate film, it becomes possible to prevent chromium from eluting into the treatment solution used for chemical conversion treatment or electrodeposition coating, which are subsequently performed on the surface-treated steel sheet. Chromium eluted from the chromate film is dissolved in the Cr in the film. 6+Therefore, in order to obtain a hardly soluble chromate film, Cr 3+ In such treatment, electrolytic chromate treatment and reactive chromate treatment are advantageous as they are likely to form a poorly soluble chromate film. However, immersion chromate treatment and paint-on chromate treatment also have the disadvantage that phosphoric acid and colloids can easily dissolve Cr. 6+ By using techniques such as fixing the surface of the material, a hardly soluble chromate film can be obtained.
[0087] Furthermore, when a so-called chromate-free coating is provided as the chemical conversion coating 40, a coating containing a resin and, if necessary, one or more selected from the group consisting of a silane coupling agent, a zirconium compound, silica, phosphoric acid and its salts, fluoride, a vanadium compound, and tannin or tannic acid may be formed. The inclusion of these substances further improves the film-forming properties after application of the chemical conversion treatment solution, the barrier properties (density) of the coating against corrosion factors such as moisture and corrosive ions, and the adhesion of the coating to the surface of the steel sheet, thereby contributing to raising the corrosion resistance of the coating.
[0088] In particular, when the chromate-free coating contains at least one of a silane coupling agent and a zirconium compound, a crosslinked structure is formed within the chromate-free coating, which also strengthens the bond with the steel sheet surface, making it possible to further improve the adhesion and barrier properties of the coating.
[0089] Furthermore, when the chromate-free coating contains one or more of silica, phosphoric acid and its salts, fluoride, and vanadium compounds, these function as inhibitors and form a precipitated film or a passive film on the surface of the steel sheet, thereby making it possible to further improve corrosion resistance.
[0090] Below, the details of each component that may be contained in the above-mentioned chromate-free coating will be explained with examples.
[0091] <<Resin>> As the resin, for example, known organic resins such as polyester resin, polyurethane resin, epoxy resin, phenolic resin, acrylic resin, polyolefin resin, etc. can be used. In order to further improve adhesion to the steel sheet, it is preferable to use at least one resin having a forced moiety or a polar functional group in the molecular chain (polyester resin, urethane resin, epoxy resin, acrylic resin, etc.). The resin may be used alone or in combination of two or more types.
[0092] The resin content in the chromate-free coating is, for example, preferably 0% by mass or more, and more preferably 1% by mass or more, relative to the coating solid content. This allows for improved corrosion resistance. Furthermore, the resin content in the chromate-free coating is, for example, preferably 85% by mass or less, more preferably 60% by mass or less, and even more preferably 40% by mass or less, relative to the coating solid content. By setting the resin content to 85% by mass or less, the corrosion resistance of the coating can be improved while ensuring the performance required of the coating other than corrosion resistance.
[0093] <Silane Coupling Agent> Examples of the silane coupling agent include γ-(2-aminoethyl)aminopropyltrimethoxysilane, γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, γ-(2-aminoethyl)aminopropyltriethoxysilane, γ-(2-aminoethyl)aminopropylmethyldiethoxysilane, γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropylmethyldimethoxysilane, γ-methacryloxypropyltriethoxysilane Silane, γ-methacryloxypropylmethyldiethoxysilane, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropylmethyldimethoxysilane, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltriethoxysilane, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropylmethyldiethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane Silane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, γ-mercaptopropyltriethoxysilane, γ-mercaptopropylmethyldiethoxysilane, methyltrimethoxysilane, dimethyldimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, vinyltriacetoxysilane, γ-chloropropyltrimethoxysilane, γ-chloropropylmethyldimethoxysilane dimethylsilane, γ-chloropropyltriethoxysilane, γ-chloropropylmethyldiethoxysilane, hexamethyldisilazane, γ-anilinopropyltrimethoxysilane, γ-anilinopropylmethyldimethoxysilane, γ-anilinopropyltriethoxysilane, γ-anilinopropylmethyldiethoxysilane, vinyltrimethoxysilane, vinylmethyldimethoxysilane, vinyltriethoxysilane, vinylmethyldiethoxysilane, octadecyldimethyl[3-(trimethoxysilyl)propyl]ammonium chloride,Examples of suitable silane coupling agents include octadecyldimethyl[3-(methyldimethoxysilyl)propyl]ammonium chloride, octadecyldimethyl[3-(triethoxysilyl)propyl]ammonium chloride, octadecyldimethyl[3-(methyldiethoxysilyl)propyl]ammonium chloride, γ-chloropropylmethyldimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, methyltrichlorosilane, dimethyldichlorosilane, and trimethylchlorosilane. The amount of silane coupling agent added to the chemical conversion treatment agent for forming a chromate-free coating can be, for example, 2 to 80 g / L. By adding 2 g / L or more of the silane coupling agent, adhesion to the steel sheet surface can be improved, thereby improving the processing adhesion of the coating. Furthermore, by adding 80 g / L or less of the silane coupling agent, the cohesive strength of the coating can be maintained, thereby improving the processing adhesion of the coating. The silane coupling agents exemplified above may be used alone or in combination of two or more.
[0094] <Zirconium Compound> Examples of zirconium compounds include zirconium normal propylate, zirconium normal butylate, zirconium tetraacetylacetonate, zirconium monoacetylacetonate, zirconium bisacetylacetonate, zirconium monoethylacetoacetate, zirconium acetylacetonate bisethylacetoacetate, zirconium acetate, zirconium monostearate, zirconium carbonate, ammonium zirconium carbonate, potassium zirconium carbonate, and sodium zirconium carbonate. The amount of zirconium compound added to a chemical conversion treatment agent for forming a chromate-free coating can be, for example, 2 to 80 g / L. By adding the zirconium compound in an amount of 2 g / L or more, adhesion to the steel sheet surface can be improved, thereby improving the processing adhesion of the coating film. Furthermore, by adding the zirconium compound in an amount of 80 g / L or less, the cohesive strength of the coating film can be maintained, thereby improving the processing adhesion of the coating film. Such zirconium compounds may be used alone or in combination of two or more.
[0095] <<Silica>> Examples of silica that can be used include commercially available silica gels such as "Snowtex N," "Snowtex C," "Snowtex UP," and "Snowtex PS" manufactured by Nissan Chemical Industries, Ltd., and "Adelite AT-20Q" manufactured by ADEKA Corporation, as well as powdered silica such as Aerosil #300 manufactured by Nippon Aerosil Co., Ltd. The type of silica can be selected appropriately depending on the required performance of the coated metal sheet. The amount of silica added to the chemical conversion treatment agent for forming a chromate-free coating is preferably 1 to 40 g / L. By adding silica in an amount of 1 g / L or more, it is possible to improve the processing adhesion of the coating film. Furthermore, by adding silica in an amount of 40 g / L or less, it is possible to achieve both processing adhesion and corrosion resistance while suppressing cost increases.
[0096] <Phosphoric Acid and Its Salts> Examples of phosphoric acid and its salts include phosphoric acids such as orthophosphoric acid, metaphosphoric acid, pyrophosphoric acid, triphosphoric acid, and tetraphosphoric acid, and salts thereof; ammonium salts such as triammonium phosphate and diammonium hydrogen phosphate; phosphonic acids such as aminotri(methylenephosphonic acid), 1-hydroxyethylidene-1,1-diphosphonic acid, ethylenediaminetetra(methylenephosphonic acid), and diethylenetriaminepenta(methylenephosphonic acid), and salts thereof; and organic phosphoric acids such as phytic acid and salts thereof. Examples of phosphoric acid salts other than ammonium salts include metal salts with Na, Mg, Al, K, Ca, Mn, Ni, Zn, Fe, and the like. Phosphoric acid and its salts may be used alone or in combination of two or more.
[0097] The content of phosphoric acid and its salts is preferably 0% by mass or more, and more preferably 1% by mass or more, based on the solid content of the coating. Furthermore, the content of phosphoric acid and its salts is preferably 20% by mass or less, and more preferably 10% by mass or less, based on the solid content of the coating. By keeping the content of phosphoric acid and its salts at 20% by mass or less, embrittlement of the coating can be prevented, and a decrease in the coating adhesion during forming of the surface-treated steel sheet can be prevented.
[0098] <Fluoride> Examples of fluorides include ammonium zirconate fluoride, ammonium silicofluoride, ammonium titanium fluoride, sodium fluoride, potassium fluoride, calcium fluoride, lithium fluoride, titanium hydrofluoric acid, zirconate hydrofluoric acid, etc. Such fluorides may be used alone or in combination of two or more.
[0099] The fluoride content is preferably 0% by mass or more, and more preferably 1% by mass or more, based on the solid content of the coating. The fluoride content is preferably 20% by mass or less, and more preferably 10% by mass or less, based on the solid content of the coating. A fluoride content of 20% by mass or less can prevent embrittlement of the coating and can prevent a decrease in the coating adhesion during forming of the surface-treated steel sheet.
[0100] <Vanadium Compound> Examples of vanadium compounds include vanadium compounds obtained by reducing pentavalent vanadium compounds such as vanadium pentoxide, metavanadic acid, ammonium metavanadate, sodium metavanadate, and vanadium oxytrichloride with a reducing agent to divalent to tetravalent vanadium compounds, and vanadium trioxide, vanadium dioxide, vanadium oxysulfate, vanadium oxyoxalate, vanadium oxyacetylacetonate, vanadium acetylacetonate, vanadium trichloride, vanadium phosphomolybdic acid, vanadium sulfate, vanadium dichloride, and vanadium oxide, and other vanadium compounds having a tetravalent to divalent oxidation number. These vanadium compounds may be used alone or in combination of two or more.
[0101] The content of the vanadium compound is preferably 0% by mass or more, and more preferably 1% by mass or more, based on the solid content of the coating. Furthermore, the content of the vanadium compound is preferably 20% by mass or less, and more preferably 10% by mass or less, based on the solid content of the coating. By keeping the vanadium compound content at 20% by mass or less, it is possible to prevent embrittlement of the coating and to prevent a decrease in the working adhesion of the coating when the surface-treated steel sheet is formed.
[0102] <Tannin or Tannic Acid> Tannin or tannic acid can be either hydrolyzable tannin or condensed tannin. Examples of tannin and tannic acid include ham meta tannin, Chinese gall tannin, gall nut tannin, myrobalan tannin, dividivi tannin, algarovila tannin, valonia tannin, and catechin. The amount of tannin or tannic acid added to the chemical conversion treatment agent for forming a chromate-free coating can be 2 to 80 g / L. By adding tannin or tannic acid in an amount of 2 g / L or more, adhesion to the steel sheet surface can be improved, thereby improving the processing adhesion of the coating film. Furthermore, by adding tannin or tannic acid in an amount of 80 g / L or less, the cohesive strength of the coating can be maintained, improving the processing adhesion of the coating film.
[0103] The thickness (d2 in FIG. 1B ) of the chemical conversion coating 40 as described above is preferably 10 to 1000 nm. By setting the thickness d2 to this value, it is possible to further improve adhesion between the coating 40 and the steel sheet 10 and between the coating 30 and corrosion resistance.
[0104] Here, the thickness d2 of the chemical conversion coating 40 can be measured by observing the vicinity of the region from the plating layer 20 to the coating film 30 using a transmission electron microscope (TEM). Such observation may be performed by observing an exposed side surface of the surface-treated steel sheet 1 in a state where the structure in the thickness direction of the surface-treated steel sheet 1 can be observed, or by observing a cross section of the surface-treated steel sheet 1 cut in the thickness direction.
[0105] Furthermore, instead of the above-described TEM observation, measurement can also be performed by radio frequency glow discharge optical emission spectroscopy (RF-GD-OES). More specifically, the presence or absence of the chemical conversion coating 40 can be confirmed based on whether or not elements that may be contained in the chemical conversion coating 40 (for example, chromium in the case of a chromate-containing coating, or elements derived from the coating other than chromium in the case of a chromate-free coating) are detected. Furthermore, the thickness of the chemical conversion coating 40 can be determined from the strength of the elements that may be contained in the chemical conversion coating 40.
[0106] When identifying the chemical conversion coating 40 from a surface-treated steel sheet that has already been processed into various parts such as a fuel tank, a test piece may be cut out from a portion of the part of interest that has not been subjected to joining processes such as welding or processing processes such as drawing or bending, and used as the object of analysis. In this case, the size of the test piece to be cut out may be the size of the test piece when it is in a flat plate form, for example, approximately 50 × 50 mm.
[0107] The surface-treated steel sheet 1 according to this embodiment has been described in detail above with reference to FIGS.
[0108] (Regarding the manufacturing method of the surface-treated steel sheet) Next, the manufacturing method of the surface-treated steel sheet according to the present embodiment as described above will be described with reference to Fig. 4. Fig. 4 is a flow chart showing an example of the flow of the manufacturing method of the surface-treated steel sheet according to the present embodiment.
[0109] As shown in FIG. 4 , the method for producing a surface-treated steel sheet according to this embodiment includes a pretreatment step (step S11), an electroplating step (step S13), a cleaning step (step S15), a chemical conversion treatment step (step S17), a cleaning step (step S19), and a coating film formation step (step S21).
[0110] The pretreatment step (step S11) is a step for cleaning the surface of the steel sheet by subjecting the steel sheet, which serves as the base material, to various pretreatments, including alkaline degreasing, water washing, pickling, etc. There are no particular restrictions on the pretreatment step, and it is sufficient to follow a conventional treatment method.
[0111] The electroplating step (step S13) is a step of forming a plating layer on the surface of a steel sheet as a base material by electroplating. In this electroplating step, a plating bath containing components capable of realizing a desired plating composition (a plating bath containing Ni and, as necessary, other elements, with the balance being Zn) is prepared, and electroplating is performed using this plating bath and the steel sheet at a predetermined current density and for a predetermined current flow time.
[0112] The plating bath temperature is preferably 50 to 70°C. The current density is preferably 5 to 100 A / dm 2 The current application time is preferably 10 to 100 seconds, and more preferably 12 to 50 seconds.
[0113] In the electroplating process (step S13) according to this embodiment, multiple cells containing the above-described plating bath are used to perform electroplating while continuously passing a steel sheet through the cells. The zinc concentration in the cells downstream in the direction of travel of the steel sheet is made higher than the zinc concentration in the cells upstream in the direction of travel. Specifically, the Zn ion concentration in the downstream cells is made to satisfy the condition that it is 1.1 times or more the average value of all plating cells. Furthermore, the current density in the downstream cells is made to satisfy the condition that it is less than 1.0 times the average value of all plating cells. Furthermore, the number of downstream cells is made to be 5% or more and 20% or less of the total number of cells. Then, the treatment is performed for the above-described current application time. This achieves the Zn concentration gradient near the interface on the coating film 30 side, as previously described.
[0114] The plating deposition amount in this electroplating step is set to 2 to 50 g / m so that the deposition amount of the plating layer 20 as previously explained can be realized. 2 It is preferable that the range is within the range.
[0115] The cleaning step (step S15) is a step of subjecting the steel sheet after the electroplating step to a cleaning treatment. The cleaning step is not particularly specified, and may be performed according to a conventional treatment method.
[0116] The chemical conversion treatment step (step S17) is a step of forming a chemical conversion coating (a chromate coating or a chromate-free coating) by subjecting the steel sheet (more specifically, the steel sheet on which the plating layer has been formed) that has been subjected to the cleaning step to a chemical conversion treatment as needed.
[0117] Such a chemical conversion treatment step may be carried out using the treatment solution as described above and in accordance with a conventional treatment method so as to achieve the thickness as described above.
[0118] The cleaning step (step S19) is a step of cleaning the steel sheet after the chemical conversion treatment step. There are no particular restrictions on the cleaning step, and the cleaning step may be performed according to a conventional treatment method.
[0119] The coating film forming step (step S21) is a step of performing a treatment for forming a coating film on the steel sheet that has been subjected to the cleaning step (more specifically, the steel sheet on which the plating layer and the chemical conversion coating have been formed).
[0120] In this process, a paint for forming the coating film is prepared so as to realize the content of the components of the coating film 30 as previously described. In such a paint, each of the components of the coating film 30 as previously described is dissolved or dispersed in an organic solvent.
[0121] In the coating film forming step according to this embodiment, it is preferable to use a ketone organic solvent as the organic solvent. By adding the ketone organic solvent to the coating material in an amount of 40 mass% or more and adjusting the coating material solids concentration to 10 to 50 mass%, it becomes possible to easily form a uniform coating film.
[0122] Examples of such ketone organic solvents include methyl isobutyl ketone, acetone cyclohexanone, isophorone, etc., but other ketone organic solvents can also be used. However, when selecting such a solvent, it is important to avoid selecting a solvent that can react with the isocyanate resin.
[0123] The paint prepared as described above is applied to the surface of the steel sheet after the cleaning process by various methods such as roll coating, curtain flow coating, etc. At this time, it is preferable to appropriately adjust the thickness of the applied paint so that the thickness of the coating film 30 after drying is within the range of 0.5 to 2.0 μm.
[0124] When applying the above-described paint, the steel sheet provided with the plating layer 20 (or the steel sheet provided with the plating layer 20 and the chemical conversion coating 40) is preheated. This preheating treatment increases the reactivity between the Si derived from the coating film 30 and the plating layer 20 or the chemical conversion coating 40, making it possible to realize the Si-enriched region described above.
[0125] The preheating temperature when applying the paint is determined depending on the temperature of the paint to be applied. More specifically, the steel sheet to be applied is preheated to a temperature that is at least 3°C higher than the temperature of the paint to be applied. The preheating temperature is preferably at least 5°C higher than the temperature of the paint to be applied.
[0126] On the other hand, if the preheating temperature of the steel sheet to be coated is too high, the drying and hardening of the paint in contact with it will be accelerated, and the components of the coating film to be applied will change. Therefore, the preheating temperature of the steel sheet to be coated should be +30°C or less higher than the temperature of the paint to be applied. The preheating temperature is preferably +20°C or less higher than the temperature of the paint to be applied.
[0127] Next, the steel sheet after coating with the paint is held, for example, at a maximum temperature in the range of 100 to 200°C for 10 to 60 seconds, thereby volatilizing the solvent in the paint and drying and solidifying the paint solids to form the coating film 30. During this heat treatment process, components contained in the paint, the chemical conversion coating, the plating layer, etc. undergo thermal diffusion, ultimately forming the Si-enriched region 50 as described above.
[0128] By going through the above steps, the surface-treated steel sheet 1 according to this embodiment as previously described is manufactured.
[0129] The method for manufacturing a surface-treated steel sheet according to this embodiment has been described in detail above with reference to FIG.
[0130] The surface-treated steel sheet according to the present invention will be specifically described below with reference to examples and comparative examples. Note that the examples shown below are merely examples of the surface-treated steel sheet according to the present invention, and the surface-treated steel sheet according to the present invention is not limited to the examples below.
[0131] (1) Zinc-nickel-plated steel sheet The plated steel sheet used was a cold-rolled steel sheet (manufactured by Nippon Steel Corporation) on which a zinc-nickel plating was formed by electroplating to achieve a predetermined nickel content. The plating weight is the plating weight per side. The plating layer of the following zinc-nickel-plated steel sheet was spray-degreased for 5 seconds using a commercially available sodium orthosilicate alkaline cleaning solution, then rinsed with water and dried. In the equipment where the above electroplating was performed, the number of downstream cells accounted for 7% of the total number of cells. The Zn concentration ratio and current density ratio of the downstream cells are shown in Tables 1-1 to 1-3 below.
[0132] (2) Chemical conversion treatment and painting treatment Chromate chemical conversion treatment solution and paint were prepared. In the chromate chemical conversion treatment, electrolytic chromate treatment was performed at a solution temperature of 50 to 70°C and a current density of 5 to 100 A / dm 2 After that, each plated steel sheet was washed with water and dried.
[0133] In addition, the following epoxy resin, isocyanate resin, silica particles, and polyethylene wax were mixed in the specified proportions to prepare paints. The contents shown in Tables 1-1 to 1-3 are the contents in the coating film (solid content).
[0134] [Epoxy Resins] Epoxy Resin A: No. 1007 manufactured by Mitsubishi Chemical Corporation, molecular weight: 2900, epoxy equivalent: 1750-2200 Epoxy Resin B: No. 827 manufactured by Mitsubishi Chemical Corporation, molecular weight: 360, epoxy equivalent: 180-190 Epoxy Resin C: No. 1001 manufactured by Mitsubishi Chemical Corporation, molecular weight: 900, epoxy equivalent: 450-500 Epoxy Resin D: H-360 manufactured by DIC Corporation, molecular weight: 25000 Epoxy Resin E: No. 4250 manufactured by Mitsubishi Chemical Corporation, molecular weight: 60000, epoxy equivalent: 7500-8900
[0135] [Isocyanate resin] Isocyanate A: hexamethylene diisocyanate manufactured by Tosoh Corporation Isocyanate B: ethyl acetoacetate block compound
[0136] [Silica particles] <Fume silica> Fumed silica A: Aerosil 300 (average particle size: 7 nm) manufactured by Nippon Aerosil Co., Ltd. Fumed silica B: Aerosil 200 (average particle size: 12 nm) manufactured by Nippon Aerosil Co., Ltd. Fumed silica C: Aerosil R972CF (average particle size: 16 nm) manufactured by Nippon Aerosil Co., Ltd. Fumed silica D: Aerosil MOX80 (average particle size: 30 nm) manufactured by Nippon Aerosil Co., Ltd. Fumed silica E: Aerosil OX50 (average particle size: 40 nm) <Colloidal silica> Colloidal silica A: Snowtex N manufactured by Nissan Chemical Co., Ltd. (average particle size: 12 nm) Colloidal silica B: Snowtex ST-NXS manufactured by Nissan Chemical Co., Ltd. (average particle size: 5 nm) Colloidal silica C: Snowtex ST-NS manufactured by Nissan Chemical Co., Ltd. (average particle size: 9 nm) Colloidal silica D: Snowtex ST-N-40 (average particle size: 22 nm) manufactured by Nissan Chemical Industries, Ltd. Colloidal silica E: Snowtex ST-YL (average particle size: 60 nm) manufactured by Nissan Chemical Industries, Ltd. Colloidal silica F: Snowtex MP-2040 (average particle size: 200 nm) manufactured by Nissan Chemical Industries, Ltd. Colloidal silica G: Snowtex MP-454M (average particle size: 450 nm) manufactured by Nissan Chemical Industries, Ltd.
[0137] [Polyethylene wax] CERIDUST 3620 manufactured by Clariant Chemicals Co., Ltd.
[0138] The paint prepared as described above was applied using a roll coater and dried and solidified by holding for 10 to 60 seconds at a maximum temperature (PMT) in the range of 165 to 185°C. The coating film thickness after drying and solidification is shown in Tables 1-1 to 1-3. The sheet temperature before application of the paint, the temperature relative to the paint, and the post-heating sheet temperature are also shown in Tables 1-1 to 1-3.
[0139] For each of the surface-treated steel sheets obtained as described above, the Zn concentration gradient and Si-enriched regions in the coating layer were measured by GD-OES using the method described above. The results obtained are shown in Tables 1-1 to 1-3.
[0140]
[0141]
[0142]
[0143] Furthermore, the corrosion resistance after processing of each of the obtained surface-treated steel sheets was evaluated from three viewpoints. The evaluation methods and evaluation criteria for each evaluation are as follows. The obtained results are summarized in Tables 2-1 to 2-3 below.
[0144] <Corrosion resistance after processing (bulge of ball head)> Test specimens were cut out from each surface-treated steel sheet, and bulged to a height of 7 mm using an Erichsen testing machine. After that, a salt spray test (JIS Z 2371:2015) was performed for 500 hours, and the area ratio of white rust on the bulge of the ball head was evaluated. The end faces and back surface were sealed before evaluation. A score of 2 or higher was considered a pass. [Evaluation criteria] Score 5: 5% or less 4: More than 5% and 7% or less 3: More than 7% and 10% or less 2: More than 10% and 12% or less 1: More than 12%
[0145] <Corrosion resistance after processing (bulge after degreasing)> Test specimens were cut out from each surface-treated steel sheet, spray-degreased using a commercially available sodium orthosilicate alkaline cleaning solution at 60°C for 2 minutes, and then bulged to a height of 7 mm using an Erichsen tester. A salt spray test (JIS Z 2371:2015) was then performed for 500 hours, and the bulge was evaluated based on the area ratio of white rust occurring on the bulge. The end faces and back surfaces were sealed before evaluation. A score of 2 or higher was considered a pass. [Evaluation criteria] Score 5: 5% or less 4: More than 5% and less than 7% 3: More than 7% and less than 10% 2: More than 10% and less than 12% 1: More than 12%
[0146] <Corrosion resistance after processing (cylindrical solvent immersion)> Test specimens were cut out from each surface-treated steel sheet and subjected to cylindrical cup drawing under the following conditions: punch diameter: 50 mmφ, punch shoulder R: 5 mm, blank diameter: 100 mmφ, drawing ratio: 2.0, and pressing pressure: 1 ton. The painted surface was the inside of the cylinder. 40 mL of the test solution below was placed in the cup of the molded product obtained by the cylindrical cup drawing, and the product was left to stand at 45°C for 1000 hours, and the pitting depth was measured. A rating of 2 or higher was considered a pass. Test liquid: Degraded gasoline + 10% aqueous solution (formic acid 100 ppm, acetic acid 200 ppm, chloride ions 100 ppm) [Evaluation criteria] Rating 5: 0.005 mm or less 4: More than 0.005 mm and less than 0.010 mm 3: More than 0.010 mm and less than 0.015 mm 2: More than 0.015 mm and less than 0.020 mm 1: More than 0.020 mm
[0147]
[0148]
[0149]
[0150] As is clear from Tables 2-1 to 2-3 above, the surface-treated steel sheets corresponding to the examples of the present invention showed pass results in each of the three types of evaluation results for corrosion resistance after processing, while some of the surface-treated steel sheets corresponding to the comparative examples of the present invention showed fail results in at least one of the three types of evaluation results for corrosion resistance after processing.
[0151] For example, in Comparative Examples Nos. 1 and 2, the conditions in the downstream cell when forming the plating layer were inappropriate, which resulted in an inappropriate Zn concentration gradient in the plating layer, and as a result, the desired post-processing corrosion resistance could not be achieved. Furthermore, in Comparative Examples Nos. 9 and 14, the preheating when forming the coating film was inappropriate, which resulted in an inappropriate concentration of Si in the coating film, and as a result, the desired post-processing corrosion resistance could not be achieved.
[0152] Although the preferred embodiments of the present invention have been described in detail above with reference to the accompanying drawings, the present invention is not limited to these examples. It is clear that a person skilled in the art to which the present invention pertains can conceive of various modifications and alterations within the scope of the technical ideas set forth in the claims, and it is understood that these also naturally fall within the technical scope of the present invention.
[0153] The embodiments disclosed herein are illustrative in all respects and are not limiting. The above-described embodiments may be omitted, substituted, or modified in various ways without departing from the scope of the appended claims, the technical scope of the present invention as described below, and the spirit thereof. For example, the components of the above-described embodiments may be arbitrarily combined within the scope that does not impair the effects of the components. Furthermore, such an arbitrary combination naturally provides the functions and effects of each of the components involved in the combination, and also provides other functions and effects that are apparent to those skilled in the art from the description of this specification.
[0154] Furthermore, the effects described in this specification are merely descriptive or exemplary and are not limiting. In other words, the technology according to the present invention may achieve other effects that will be apparent to those skilled in the art from the description of this specification, in addition to or in place of the above-described effects.
[0155] The following configurations also fall within the technical scope of the present invention. (1) A surface-treated steel sheet comprising: a zinc- and nickel-containing plating layer located on at least one surface of a steel sheet; and a coating film located on the plating layer and containing at least an epoxy resin and an isocyanate resin, wherein, when a cross section cut in the thickness direction after being subjected to a 10% tensile elongation is observed, within a region 60 μm long in a direction perpendicular to the thickness direction, the ratio of the total length of cracks generated in the coating film to the total length of cracks generated in the plating layer is 80% or less. (2) A surface-treated steel sheet according to (1), wherein a Si-enriched region is present at the interface between the chemical conversion coating and the coating film, and wherein the plating layer has a concentration gradient in which the Zn concentration at the interface on the coating film side is higher than the Zn concentration at the interface on the plating layer side. (3) A surface-treated steel sheet according to (1) or (2), wherein the coating film has a thickness of 0.5 to 2.0 μm. (4) The surface-treated steel sheet according to any one of (1) to (3), wherein the epoxy resin is a bisphenol A-type epoxy resin having a number-average molecular weight of 300 to 100,000. (5) The surface-treated steel sheet according to (4), wherein the coating film further contains silica particles. (6) The surface-treated steel sheet according to (5), wherein the coating film further contains polyethylene wax, wherein the content of the epoxy resin is 30.0 mass% or more relative to the coating film solid content, the content of the isocyanate resin is 0.1 to 2.0 mass% relative to the epoxy resin, the content of the silica particles is 5.0 to 50.0 mass% relative to the coating film solid content, and the content of the polyethylene wax is 0.1 to 10.0 mass% relative to the coating film solid content, and the coating film contains the epoxy resin, the isocyanate resin, the silica particles, and the polyethylene wax in a total amount of 100 mass% or less. (7) The surface-treated steel sheet according to (5) or (6), wherein the silica particles are at least either fumed silica or colloidal silica, the fumed silica has an average particle size of 5 to 40 nm, and the colloidal silica has an average particle size of 5 to 200 nm.(8) The surface-treated steel sheet according to any one of (1) to (7), further comprising a chemical conversion coating between the plating layer and the paint film, the chemical conversion coating having a thickness of 10 to 1000 nm. (9) The surface-treated steel sheet according to any one of (1) to (8), which is used as a material for a fuel tank.
[0156] REFERENCE SIGNS LIST 1 Surface-treated steel sheet 10 Steel sheet 20 Plating layer 30 Paint film 40 Chemical conversion coating 50 Si-enriched region
Claims
1. A surface-treated steel sheet comprising: a plating layer containing zinc and nickel located on at least one surface of the steel sheet; and a coating film located on the plating layer and containing at least an epoxy resin and an isocyanate resin; and when a cross section cut in the thickness direction after being subjected to a tensile elongation of 10%, is observed, within a region 60 μm long in a direction perpendicular to the thickness direction, the ratio of the total length of cracks generated in the coating film to the total length of cracks generated in the plating layer is 80% or less.
2. The surface-treated steel sheet according to claim 1, wherein a Si-enriched region in which Si is concentrated is present at the interface between the plating layer and the coating film, and the plating layer has a concentration gradient in which the Zn concentration at the interface on the coating film side is higher than the Zn concentration at the interface on the plating layer side.
3. The surface-treated steel sheet according to claim 1 or 2, wherein the coating film has a thickness of 0.5 to 2.0 μm.
4. The surface-treated steel sheet according to claim 1 or 2, wherein the epoxy resin is a bisphenol A type epoxy resin having a number average molecular weight of 300 to 100,000.
5. The surface-treated steel sheet according to claim 4, wherein the coating further contains silica particles.
6. The surface-treated steel sheet according to claim 5, wherein the coating further contains polyethylene wax, the epoxy resin content is 30.0 mass% or more relative to the coating solid content, the isocyanate resin content is 0.1 to 2.0 in terms of mass ratio relative to the epoxy resin, the silica particle content is 5.0 to 50.0 mass% relative to the coating solid content, and the polyethylene wax content is 0.1 to 10.0 mass% relative to the coating solid content, and the coating contains the epoxy resin, the isocyanate resin, the silica particles, and the polyethylene wax in a total amount of 100 mass% or less.
7. The surface-treated steel sheet according to claim 5 or 6, wherein the silica particles are at least one of fumed silica and colloidal silica, the average particle size of the fumed silica is 5 to 40 nm, and the average particle size of the colloidal silica is 5 to 200 nm.
8. The surface-treated steel sheet according to claim 1 or 2, further comprising a chemical conversion coating between the plating layer and the paint film, the chemical conversion coating having a thickness of 10 to 1000 nm.
9. The surface-treated steel sheet according to claim 1 or 2, which is used as a material for a fuel tank.
Citation Information
Patent Citations
Precoated galvanized steel sheet having excellent workability and corrosion resistance of worked portion
JP2003277903A
Weldable surface-treated steel sheet with high corrosion resistance for automobile, and manufacturing method therefor
JP2005325427A
Coated steel sheet whose processing part is excellent in corrosion resistance
JP2008254349A
Clear coated steel sheet excellent in corrosion resistance of worked part
JP2009241495A
Corrosion-resistant member for biofuel
JP2011026669A