Adhesive, adhesive sheet, optical component, and display

The adhesive with an oxygen absorber addresses the issue of needle-like cracks and light reflection losses by capturing oxygen and stabilizing the adhesive layer under UV exposure, enhancing the weather resistance and image quality of display modules.

WO2024204744A1PCT designated stage expired Publication Date: 2024-10-03LINTEC CORP

Patent Information

Application Number
PCT/JP2024/013110
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

The use of air layers between protective panels and display modules in mobile electronic devices leads to significant light reflection losses due to refractive index differences, resulting in deteriorated image quality, and existing adhesive solutions are prone to needle-shaped cracks when exposed to high-intensity ultraviolet radiation, particularly during accelerated weather resistance tests.

Method used

An adhesive containing an oxygen absorber, specifically a compound represented by general formula (I) or (II), is used to suppress the formation of needle-like cracks and enhance weather resistance by capturing oxygen and preventing structural changes that lead to cracking, even under prolonged high-intensity ultraviolet exposure.

Benefits of technology

The adhesive effectively prevents the occurrence of needle-like cracks and maintains excellent weather resistance, ensuring improved image quality and durability of display modules by stabilizing the adhesive layer's structure under UV exposure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013110_03102024_PF_FP_ABST
    Figure JP2024013110_03102024_PF_FP_ABST
Patent Text Reader

Abstract

An adhesive according to the present invention is for optical applications and contains an oxygen absorber. The adhesive has excellent weather resistance and can suppress the occurrence of needle-like cracks. The oxygen absorber is preferably a compound represented by general formula (II). (In general formula (II), R9 represents a hydrogen atom or a methyl group, and R10 represents a hydroxyl group, a (meth)acryloyloxy group, a styryloxy group, or a C2–5 alkenyloxy group. R11, R12, R13, and R14 each independently represent a C1–6 alkyl group, a C2–6 alkenyl group, an aryl group, or an aralkyl group.)
Need to check novelty before this filing date? Find Prior Art

Description

Adhesive, adhesive sheet, optical structure and display

[0001] The present invention relates to an adhesive and an adhesive sheet, as well as an optical construction and a display obtained by using the same.

[0002] BACKGROUND ART In recent years, various mobile electronic devices such as mobile phones, smartphones, and tablet terminals are equipped with displays that use display modules having liquid crystal elements, light-emitting diodes (LED elements), organic electroluminescence (organic EL) elements, etc.

[0003] In such displays, a protective panel is usually provided on the front side of the display module. As electronic devices become thinner and lighter, the protective panel is increasingly being replaced by a plastic plate such as an acrylic plate or a polycarbonate plate, rather than the conventional glass plate.

[0004] Here, a gap is provided between the protective panel and the display module so that even when the protective panel is deformed by an external force, the deformed protective panel will not collide with the display module.

[0005] However, when such a gap, i.e., an air layer, is present, there is a problem that the difference in refractive index between the protective panel and the air layer, and the difference in refractive index between the air layer and the display module, results in a large light reflection loss, which reduces the image quality of the display.

[0006] Therefore, it has been proposed to improve the image quality of a display by filling the gap between the protective panel and the display module with an adhesive layer (pressure-sensitive adhesive layer). For example, Patent Document 1 discloses a pressure-sensitive adhesive layer having a shear storage modulus (G') of 1.0 x 10 at 25°C and 1 Hz, which is used to fill the gap between the protective panel and the display module. 5 The document discloses a pressure-sensitive adhesive layer having a viscosity of 100 Pa or less and a gel fraction of 40% or more.

[0007] JP 2010-97070 A

[0008] However, when a display obtained using the above adhesive layer is irradiated with high-intensity ultraviolet light for a long period of time, needle-like cracks may occur in the adhesive layer. This problem is particularly likely to occur when an accelerated weather resistance test is performed in which high-intensity ultraviolet light is irradiated for a long period of time.

[0009] The present invention has been made in consideration of the above-described circumstances, and aims to provide an adhesive, adhesive sheet, optical structure, and display that can suppress the occurrence of needle-like cracks and have excellent weather resistance.

[0010] In order to achieve the above object, first, the present invention provides an adhesive for optical applications, which contains an oxygen absorber (Invention 1).

[0011] The oxygen absorber contained in the adhesive according to the above invention (Invention 1) can capture oxygen derived from the adhesive, the adherend, the lamination process, etc. As a result, the adhesive is prevented from undergoing structural changes (e.g., destruction of crosslinking points) that could lead to needle-like cracks, even when irradiated with high-intensity ultraviolet light for a long period of time (e.g., 20 hours, 40 hours, 80 hours, etc.). As a result, the occurrence of needle-like cracks can be suppressed, and excellent weather resistance can be achieved.

[0012] In the above invention (Invention 1), the oxygen absorber is preferably a compound represented by the following general formula (I) (Invention 2). (In general formula (I), X and Y each independently represent a chalcogen atom, and R 1 , R 2 , R 7 , and R 8 each independently represents an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an aryl group, or an aralkyl group; R 3 , R 4 , R 5 , and R 6each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an aryl group, or an aralkyl group. J represents a linking group made of an aliphatic hydrocarbon having 3 to 15 carbon atoms, and any carbon atom in the linking group may be substituted with an oxygen atom, and the linking group may have at least one substituent selected from the group consisting of a hydroxyl group, a (meth)acryloyloxy group, a styryloxy group, and an alkenyloxy group having 2 to 5 carbon atoms. n is an integer from 1 to 5. However, Y, R 5 , R 6 , R 7 , and R 8 When there are a plurality of groups, they may be different atoms or groups.

[0013] In the above inventions (Inventions 1 and 2), the oxygen absorber is preferably a compound represented by the following general formula (II) (Invention 3). (In general formula (II), R 9 represents a hydrogen atom or a methyl group, R 10 represents a hydroxyl group, a (meth)acryloyloxy group, a styryloxy group, or an alkenyloxy group having 2 to 5 carbon atoms. 11 , R 12 , R 13 , and R 14 each independently represents an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an aryl group, or an aralkyl group.

[0014] In the above inventions (Inventions 1 to 3), the oxygen absorber is preferably a compound represented by the following formula (III) (Invention 4).

[0015] In the above inventions (Inventions 1 to 4), an acrylic adhesive is preferred (Invention 5).

[0016] In the above inventions (Inventions 1 to 5), the main adhesive agent is preferably a (meth)acrylic acid ester polymer or a crosslinked product thereof (Invention 6).

[0017] In the above inventions (Inventions 1 to 6), the adhesive is preferably an active energy ray-curable adhesive (Invention 7).

[0018] Secondly, the present invention provides an adhesive sheet having an adhesive layer for bonding two members together, wherein at least one of the members is an optical member, and the adhesive layer is made of any of the adhesives (Inventions 1 to 7) (Invention 8).

[0019] In the above invention (Invention 8), the chromaticity b* of the adhesive layer after lamination, as defined by the CIE 1976 L*a*b* color system, is b*1, and the illuminance of the adhesive layer after lamination is 100 mW / cm 2 When the chromaticity b* of the adhesive layer defined by the CIE 1976 L*a*b* color system is b*2 after 120 hours of irradiation with ultraviolet light, it is preferable that the absolute value of the ratio of b*2 to b*1 is 10 or less (Invention 9).

[0020] In the above inventions (Inventions 8 and 9), it is preferable that the adhesive sheet has two release sheets, and the adhesive layer is sandwiched between the release sheets so as to contact the release surfaces of the two release sheets (Invention 10).

[0021] Thirdly, the present invention provides an optical construct comprising at least two members bonded together by an adhesive layer, wherein at least one of the members is an optical member, and the adhesive layer is formed from any of the adhesives (Inventions 1 to 7) (Invention 11).

[0022] Fourth, the present invention provides a display comprising one display component, another display component, and an adhesive layer for bonding the one display component and the other display component to each other, wherein the adhesive layer is formed from the adhesive layer of the adhesive sheet (Inventions 8 to 10) (Invention 12).

[0023] In the above invention (Invention 12), both the one display member and the other display member may be hard plates (Invention 13).

[0024] The adhesive, adhesive sheet, optical construction, and display according to the present invention can suppress the occurrence of needle-like cracks and have excellent weather resistance.

[0025] 1 is a cross-sectional view of an adhesive sheet according to one embodiment of the present invention;

[0026] Hereinafter, an embodiment of the present invention will be described. [Adhesive] An adhesive according to one embodiment of the present invention is used for optical purposes and preferably contains an oxygen absorber. Generally, an adhesive is used in high illuminance (for example, 100 mW / cm 2 It is believed that prolonged irradiation with ultraviolet light of this intensity causes changes in the crosslinking structure of the adhesive, resulting in the formation of needle-like cracks. In contrast, the adhesive according to this embodiment contains an oxygen absorber, which captures oxygen derived from the adhesive, the adherend, the lamination process, etc., thereby suppressing changes in the crosslinking structure of the adhesive even after prolonged irradiation with high-intensity ultraviolet light (e.g., 20 hours, 40 hours, 80 hours, etc.). As a result, structural changes that could serve as starting points for needle-like cracks (e.g., destruction of crosslinking points) are suppressed. In this way, the adhesive according to this embodiment can suppress the occurrence of needle-like cracks and has excellent weather resistance.

[0027] The oxygen absorber in this embodiment is preferably a compound represented by the following general formula (I) (hereinafter, sometimes referred to as "compound Q"). (In general formula (I), X and Y each independently represent a chalcogen atom, and R 1 , R 2 , R 7 , and R 8 each independently represents an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an aryl group, or an aralkyl group; R 3 , R 4 , R 5 , and R 6each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an aryl group, or an aralkyl group. J represents a linking group made of an aliphatic hydrocarbon having 3 to 15 carbon atoms, and any carbon atom in the linking group may be substituted with an oxygen atom, and the linking group may have at least one substituent selected from the group consisting of a hydroxyl group, a (meth)acryloyloxy group, a styryloxy group, and an alkenyloxy group having 2 to 5 carbon atoms. n is an integer from 1 to 5. However, Y, R 5 , R 6 , R 7 , and R 8 When there are a plurality of groups, they may be different atoms or groups.

[0028] In general formula (I), n is preferably 1 to 4, more preferably 1 or 2, from the viewpoint of easy availability of raw materials.

[0029] In general formula (I), X and Y are preferably an oxygen atom or a sulfur atom, more preferably an oxygen atom, from the viewpoint of ease of production of compound Q and of improving oxygen absorption performance.

[0030] R in general formula (I) 1 , R 2 , R 7 , and R 8 Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an isopentyl group, a neopentyl group, an n-hexyl group, a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, and a cyclohexyl group.

[0031] R in general formula (I) 1 , R 2 , R 7 , and R 8 Examples of the alkenyl group having 2 to 6 carbon atoms include a vinyl group, an allyl group, a propenyl group, an isopropenyl group, a butenyl group, an isobutenyl group, a pentenyl group, a heptenyl group, a hexenyl group, an iso-3-hexenyl group, and a cyclohexenyl group.

[0032] R in general formula (I)1 , R 2 , R 7 , and R 8 Examples of the aryl group include a phenyl group, a tolyl group, a xylyl group, and a naphthyl group.

[0033] R in general formula (I) 1 , R 2 , R 7 , and R 8 Examples of the aralkyl group include a benzyl group, a 2-phenylethyl group, a 2-naphthylethyl group, and a diphenylmethyl group.

[0034] Among the above, R 1 , R 2 , R 7 , and R 8 are each independently preferably either an alkyl group having 1 to 6 carbon atoms or an alkenyl group having 2 to 6 carbon atoms, more preferably an alkyl group having 1 to 4 carbon atoms, and even more preferably a methyl group.

[0035] R in general formula (I) 3 , R 4 , R 5 , and R 6 The alkyl group having 1 to 6 carbon atoms, the alkenyl group having 2 to 6 carbon atoms, the aryl group, and the aralkyl group are the same as those in the above R 1 , R 2 , R 7 , and R 8 Examples of the alkyl group include the alkyl group having 2 to 6 carbon atoms, the alkenyl group having 2 to 6 carbon atoms, the aryl group, and the aralkyl group.

[0036] Among the above, R 3 , R 4 , R 5 , and R 6 are each independently preferably any one of a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, an alkenyl group having 2 or 3 carbon atoms, and an aryl group, more preferably a hydrogen atom or a methyl group, and even more preferably a hydrogen atom. 3 and R 6 are preferably all hydrogen atoms, and R 4 and R5 are each preferably independently a hydrogen atom or a methyl group, and more preferably all are a hydrogen atom.

[0037] In general formula (I), the linking group of J is preferably an aliphatic hydrocarbon group having 3 to 10 carbon atoms, and more preferably an aliphatic hydrocarbon group having 3 to 5 carbon atoms, from the viewpoint of ease of handling of compound Q. Examples of styryloxy groups which are optional substituents on the linking group of J include 4-styryloxy groups. Furthermore, the alkenyloxy group having 2 to 5 carbon atoms which is optional substituent on the linking group of J may be a vinyloxy group having 2 to 5 carbon atoms. From the viewpoint of improving the oxygen absorption performance of compound Q, the optional substituent on the linking group of J is preferably a hydroxyl group or a (meth)acryloyloxy group.

[0038] As a specific example of the linking group of J, a linking group represented by the following general formula (J-1) is more preferred from the viewpoint of improving the oxygen absorption performance of compound Q. In addition, "*" in general formula (J-1) indicates the point of attachment to X or Y. In the above general formula (J-1), R 9 represents a hydrogen atom or a methyl group, and is preferably a hydrogen atom. 10 represents any one of a hydroxyl group, a (meth)acryloyloxy group, a styryloxy group, and an alkenyloxy group having 2 to 5 carbon atoms, and is preferably a hydroxyl group or a (meth)acryloyloxy group. The alkenyloxy group having 2 to 5 carbon atoms may be a vinyloxy group having 2 to 5 carbon atoms.

[0039] As a specific example of the compound Q, a compound represented by the following general formula (II) is preferred from the viewpoint of oxygen absorption performance. (In general formula (II), R 9 represents a hydrogen atom or a methyl group, R 10 represents a hydroxyl group, a (meth)acryloyloxy group, a styryloxy group, or an alkenyloxy group having 2 to 5 carbon atoms. 11 , R 12 , R 13 , and R 14each independently represents an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an aryl group, or an aralkyl group.

[0040] R in general formula (II) 10 is preferably a hydroxyl group or a (meth)acryloyloxy group. 10 The alkenyloxy group having 2 to 5 carbon atoms may be a vinyloxy group having 2 to 5 carbon atoms.

[0041] R in general formula (II) 11 , R 12 , R 13 , and R 14 The preferred embodiments of the above are R 1 , R 2 , R 7 , and R 8 is the same as

[0042] The oxygen absorber in this embodiment is particularly preferably a compound represented by the following formula (III) (hereinafter sometimes referred to as "compound S").

[0043] The method for producing compound Q is not particularly limited, and compound Q can be produced by using a known method or by combining and applying known methods. As an example, compound S can be produced by reacting 3-methyl-2-buten-1-ol with a compound capable of forming linking group J, such as epichlorohydrin, in the presence of an alkali such as potassium hydroxide. As reaction conditions, from the viewpoint of ensuring a sufficient reaction, it is preferable to stir the mixture at a temperature of about 25 to 70°C for about 2 to 10 hours.

[0044] The content of the oxygen absorber in the adhesive according to this embodiment is preferably 0.01 to 20% by mass, more preferably 0.05 to 12% by mass, particularly preferably 0.1 to 8% by mass, even more preferably 0.4 to 4% by mass, and most preferably 0.8 to 2% by mass. This makes it possible to more effectively suppress the occurrence of needle-like cracks, and achieves better weather resistance.

[0045] The adhesive according to this embodiment is preferably a pressure-sensitive adhesive (adhesive), but is not limited to this. The type of adhesive according to this embodiment may be any of an acrylic adhesive, a polyester adhesive, a polyurethane adhesive, a rubber adhesive, a silicone adhesive, etc. Furthermore, the adhesive may be any of an emulsion type, a solvent type, or a solventless type, and may be either a crosslinked type or a non-crosslinked type. Among these, an acrylic adhesive is preferred because of its excellent pressure-sensitive adhesive properties, optical properties, etc.

[0046] The acrylic adhesive may be an active energy ray-curable adhesive, an active energy ray-non-curable adhesive, a crosslinkable adhesive, a non-crosslinkable adhesive, or a combination thereof. Among these, an active energy ray-curable acrylic adhesive is preferred from the viewpoint of easily obtaining excellent weather resistance.

[0047] From the viewpoint of film-forming properties, the adhesive according to this embodiment preferably contains a (meth)acrylic acid ester polymer as the main adhesive agent, and particularly preferably contains a crosslinked (meth)acrylic acid ester polymer. The adhesive according to this embodiment also preferably contains the main adhesive agent and an active energy ray-curable component. The crosslinked (meth)acrylic acid ester polymer is preferably a crosslinked (meth)acrylic acid ester polymer and a crosslinking agent.

[0048] Specifically, the adhesive according to this embodiment is preferably obtained by crosslinking (preferably thermally crosslinking) an adhesive composition (hereinafter sometimes referred to as "adhesive composition P") containing a (meth)acrylic acid ester polymer (A), a crosslinking agent (B), an oxygen absorber (C), and, if desired, an active energy ray-curable component (D). In this specification, (meth)acrylic acid refers to both acrylic acid and methacrylic acid. The same applies to other similar terms. Furthermore, the term "polymer" also includes the concept of "copolymer."

[0049] (1) Components (1-1) (Meth)acrylic acid ester polymer (A) The (meth)acrylic acid ester polymer (A) preferably contains a structural unit derived from a (meth)acrylic acid alkyl ester. This allows the polymer to exhibit good pressure-sensitive adhesive properties. Note that the (meth)acrylic acid alkyl ester does not include the hard monomers described below.

[0050] From the viewpoint of pressure-sensitive adhesiveness, the (meth)acrylic acid alkyl ester is preferably a (meth)acrylic acid alkyl ester having an alkyl group containing 1 to 20 carbon atoms. Examples of (meth)acrylic acid alkyl esters having an alkyl group containing 1 to 20 carbon atoms include methyl acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, myristyl (meth)acrylate, palmityl (meth)acrylate, and stearyl (meth)acrylate. These may be used alone or in combination of two or more. Among the above, from the viewpoint of further improving pressure-sensitive adhesiveness, (meth)acrylic acid esters in which the alkyl group has 1 to 14 carbon atoms are preferred, (meth)acrylic acid esters in which the alkyl group has 2 to 10 carbon atoms are more preferred, and (meth)acrylic acid esters in which the alkyl group has 3 to 8 carbon atoms are particularly preferred. Specifically, for example, methyl acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, or isooctyl (meth)acrylate are preferred, n-butyl acrylate or 2-ethylhexyl acrylate are particularly preferred, and 2-ethylhexyl acrylate is even more preferred.

[0051] From the viewpoint of imparting pressure-sensitive adhesiveness, the (meth)acrylic acid ester polymer (A) preferably contains 30 to 99 mass %, more preferably 40 to 92 mass %, particularly preferably 50 to 86 mass %, even more preferably 55 to 80 mass %, and of these, preferably 60 to 75 mass %, of structural units derived from a (meth)acrylic acid alkyl ester.

[0052] The (meth)acrylic acid ester polymer (A) preferably contains a structural unit derived from a reactive functional group-containing monomer, whereby the reactive functional group derived from the reactive functional group-containing monomer reacts with the crosslinking agent (B) to form a crosslinked structure (three-dimensional network structure), thereby obtaining an adhesive having the desired cohesive strength.

[0053] Preferred examples of the reactive group-containing monomer include a monomer having a hydroxyl group in the molecule (hydroxyl group-containing monomer), a monomer having a carboxyl group in the molecule (carboxyl group-containing monomer), a monomer having an amino group in the molecule (amino group-containing monomer), etc. Among these, a hydroxyl group-containing monomer or a carboxyl group-containing monomer, which has excellent reactivity with the crosslinking agent (B), is preferred.

[0054] Examples of hydroxyl group-containing monomers include (meth)acrylic acid hydroxyalkyl esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. Among these, 2-hydroxyethyl (meth)acrylate or 4-hydroxybutyl (meth)acrylate is preferred from the viewpoints of reactivity with the crosslinking agent (B) and copolymerizability with other monomers. These may be used alone or in combination of two or more.

[0055] Examples of carboxyl group-containing monomers include ethylenically unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, itaconic acid, and citraconic acid. Among them, acrylic acid or methacrylic acid is preferred, and acrylic acid is particularly preferred, from the viewpoint of reactivity with the crosslinking agent (B) and copolymerizability with other monomers. These may be used alone or in combination of two or more.

[0056] From the viewpoint of cohesive strength, the content of the structural unit derived from the reactive functional group-containing monomer in the (meth)acrylic acid ester polymer (A) is preferably 1 to 40 mass%, more preferably 3 to 34 mass%, particularly preferably 6 to 28 mass%, even more preferably 9 to 24 mass%, and of these, preferably 12 to 20 mass%.

[0057] The (meth)acrylic acid ester polymer (A) also preferably contains a structural unit derived from a hard monomer having a glass transition temperature (Tg) of 70°C or higher as a homopolymer. The aforementioned reactive functional group-containing monomers are excluded from the hard monomer. When the (meth)acrylic acid ester polymer (A) contains a structural unit derived from the hard monomer, the resulting adhesive has improved cohesive strength and is more likely to exhibit excellent blister resistance. In particular, when the (meth)acrylic acid ester polymer (A) contains a structural unit derived from a (meth)acrylic acid ester having an alkyl group with 5 to 8 carbon atoms, the cohesive strength tends to be low, so it is preferable to contain the structural unit derived from the hard monomer. The glass transition temperature (Tg) of the hard monomer as a homopolymer is preferably 75 to 200°C, more preferably 80 to 180°C, and even more preferably 90 to 150°C.

[0058] Examples of the hard monomer include methyl methacrylate (Tg 105° C.), isobornyl acrylate (Tg 94° C.), isobornyl methacrylate (Tg 180° C.), adamantyl acrylate (Tg 115° C.), adamantyl methacrylate (Tg 141° C.), etc. These may be used alone or in combination of two or more.

[0059] Among the above hard monomers, from the viewpoint of better exhibiting the performance of the hard monomer while preventing adverse effects on other properties such as pressure-sensitive adhesiveness and transparency, methyl methacrylate or isobornyl acrylate is more preferred, and isobornyl acrylate, which is a monomer having an alicyclic structure in the molecule (alicyclic structure-containing monomer), is particularly preferred.

[0060] When the (meth)acrylic acid ester polymer (A) contains the structural unit derived from the hard monomer, the content thereof is preferably 1 to 30 mass%, more preferably 4 to 25 mass%, particularly preferably 8 to 20 mass%, and even more preferably 10 to 16 mass%, from the viewpoints of cohesive strength and blister resistance.

[0061] The (meth)acrylic acid ester polymer (A) also preferably contains a structural unit derived from a monomer having a nitrogen atom in the molecule (nitrogen atom-containing monomer). In particular, when an alicyclic structure-containing monomer, particularly isobornyl acrylate, is used as the hard monomer, it is preferable to contain a structural unit derived from a nitrogen atom-containing monomer. The presence of a structural unit derived from a nitrogen atom-containing monomer can impart a predetermined polarity to the adhesive and improve adhesion.

[0062] As the nitrogen atom-containing monomer, a monomer having a nitrogen-containing heterocycle is preferred from the viewpoint of imparting appropriate rigidity to the (meth)acrylic acid ester polymer (A). Also, from the viewpoint of increasing the degree of freedom of the nitrogen atom-containing monomer-derived portion in the higher-order structure of the resulting adhesive, it is preferred that the nitrogen atom-containing monomer does not contain a reactive unsaturated double bond group other than one polymerizable group used in polymerization to form the (meth)acrylic acid ester polymer (A).

[0063] Examples of monomers having a nitrogen-containing heterocycle include N-(meth)acryloylmorpholine, N-vinyl-2-pyrrolidone, N-(meth)acryloylpyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-(meth)acryloylaziridine, aziridinylethyl (meth)acrylate, 2-vinylpyridine, 4-vinylpyridine, 2-vinylpyrazine, 1-vinylimidazole, N-vinylcarbazole, and N-vinylphthalimide. Among these, N-(meth)acryloylmorpholine, which exhibits superior adhesive strength, is preferred, and N-acryloylmorpholine is particularly preferred. These may be used alone or in combination of two or more.

[0064] When the (meth)acrylic acid ester polymer (A) contains a structural unit derived from a nitrogen atom-containing monomer, the content thereof is preferably 1 to 20 mass%, more preferably 2 to 16 mass%, particularly preferably 3 to 12 mass%, and even more preferably 4 to 8 mass%, from the viewpoint of better adhesiveness.

[0065] The (meth)acrylic acid ester polymer (A) may contain structural units derived from other monomers, if desired. The other monomers are preferably monomers that do not contain reactive functional groups, so as not to interfere with the action of the reactive group-containing monomer. Examples of such other monomers include (meth)acrylic acid alkoxyalkyl esters such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate, vinyl acetate, and styrene. These may be used alone or in combination of two or more.

[0066] The (meth)acrylic acid ester polymer (A) may be a solution polymerized product, a solvent-free polymerized product, or an emulsion polymerized product. Among these, a solution polymer obtained by solution polymerization is preferred. By using a solution polymer, a high molecular weight polymer can be easily obtained, and better weather resistance can be easily obtained.

[0067] The polymerization mode of the (meth)acrylic acid ester polymer (A) may be a random copolymer or a block copolymer.

[0068] The weight average molecular weight of the (meth)acrylic acid ester polymer (A) is preferably 100,000 to 3,000,000, more preferably 200,000 to 2,400,000, particularly preferably 300,000 to 1,800,000, even more preferably 400,000 to 1,200,000, and most preferably 450,000 to 800,000. This makes it easier to obtain better weather resistance. Note that the weight average molecular weight in this specification is a value measured by gel permeation chromatography (GPC) in terms of standard polystyrene.

[0069] In the adhesive composition P, the (meth)acrylic acid ester polymer (A) may be used alone or in combination of two or more.

[0070] The content of the (meth)acrylic acid ester polymer (A) in the adhesive composition P according to this embodiment is preferably 70 to 99.9% by mass, more preferably 80 to 99% by mass, particularly preferably 85 to 98% by mass, and even more preferably 90 to 97% by mass. This makes it possible to obtain an adhesive having excellent film-forming properties and pressure-sensitive adhesive properties, and to easily obtain even better weather resistance.

[0071] (1-2) Crosslinking Agent (B) The crosslinking agent (B) crosslinks the (meth)acrylic acid ester polymer (A) by heating the adhesive composition P, making it possible to favorably form a crosslinked structure having a three-dimensional network structure. This makes it possible to obtain an adhesive having a predetermined cohesive strength and to easily obtain better weather resistance.

[0072] The crosslinking agent (B) may be any agent that reacts with the reactive functional group (hydroxyl group or carboxyl group) of the (meth)acrylic acid ester polymer (A), and examples thereof include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, amine-based crosslinking agents, melamine-based crosslinking agents, aziridine-based crosslinking agents, hydrazine-based crosslinking agents, aldehyde-based crosslinking agents, oxazoline-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, and ammonium salt-based crosslinking agents. When the (meth)acrylic acid ester polymer (A) contains a structural unit derived from a hydroxyl group-containing monomer, it is preferable to use an isocyanate-based crosslinking agent that has excellent reactivity with hydroxyl groups as the crosslinking agent (B). The crosslinking agent (B) may be used alone or in combination of two or more.

[0073] The isocyanate-based crosslinking agent contains at least a polyisocyanate compound. Examples of polyisocyanate compounds include aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, and xylylene diisocyanate; aliphatic polyisocyanates such as hexamethylene diisocyanate; alicyclic polyisocyanates such as isophorone diisocyanate and hydrogenated diphenylmethane diisocyanate; and biuret and isocyanurate forms thereof, as well as adducts thereof that are reaction products with low-molecular-weight active hydrogen-containing compounds such as ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, and castor oil. Among these, trimethylolpropane-modified aromatic polyisocyanates, particularly trimethylolpropane-modified tolylene diisocyanate or trimethylolpropane-modified xylylene diisocyanate, are preferred from the viewpoint of reactivity with hydroxyl groups.

[0074] The content of the crosslinking agent (B) in the adhesive composition P is preferably 0.01 to 10 parts by mass, more preferably 0.04 to 5 parts by mass, particularly preferably 0.08 to 1 part by mass, even more preferably 0.12 to 0.6 parts by mass, and especially preferably 0.15 to 0.3 parts by mass, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). This makes it easier to obtain better weather resistance.

[0075] (1-3) Oxygen Absorber (C) The oxygen absorber (C) used in the adhesive composition P is the oxygen absorber described above, and its specific components and content (mass %) in the adhesive are as described above. The amount of the oxygen absorber (C) in the adhesive composition P relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A) is preferably 0.01 to 20 parts by mass, more preferably 0.05 to 15 parts by mass, particularly preferably 0.1 to 10 parts by mass, even more preferably 0.4 to 5 parts by mass, and of these, preferably 0.8 to 2 parts by mass. This makes it possible to more effectively suppress the occurrence of needle-like cracks, and to obtain better weather resistance.

[0076] (1-4) Active energy ray-curable component (D) When the adhesive composition P contains the active energy ray-curable component (D), the resulting adhesive is active energy ray-curable. The active energy ray-cured adhesive layer can easily achieve better weather resistance by active energy ray curing after lamination.

[0077] The active energy ray-curable component (D) is not particularly limited as long as it is a component that can be cured by irradiation with active energy rays without impairing adhesiveness, and may be any of a monomer, an oligomer, a polymer, or a mixture thereof. Among them, a polyfunctional acrylate-based monomer is preferred, as it can easily provide better weather resistance.

[0078] Examples of polyfunctional acrylate monomers include bifunctional monomers such as 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, neopentyl glycol adipate di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, caprolactone-modified dicyclopentenyl di(meth)acrylate, ethylene oxide-modified phosphate di(meth)acrylate, di(acryloxyethyl)isocyanurate, allylated cyclohexyl di(meth)acrylate, ethoxylated bisphenol A diacrylate, and 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene; trifunctional types such as diglycerol tetra(meth)acrylate and pentaerythritol tetra(meth)acrylate; pentafunctional types such as propionic acid-modified dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide-modified trimethylolpropane tri(meth)acrylate, tris(acryloxyethyl)isocyanurate, and ε-caprolactone-modified tris-(2-(meth)acryloxyethyl)isocyanurate; tetrafunctional types such as diglycerol tetra(meth)acrylate and pentaerythritol tetra(meth)acrylate; pentafunctional types such as propionic acid-modified dipentaerythritol penta(meth)acrylate; and hexafunctional types such as dipentaerythritol hexa(meth)acrylate and caprolactone-modified dipentaerythritol hexa(meth)acrylate. Among the above, from the viewpoint of the weather resistance of the resulting adhesive, polyfunctional acrylate monomers containing an isocyanurate structure in the molecule, such as di(acryloxyethyl)isocyanurate, tris(acryloxyethyl)isocyanurate, and ε-caprolactone-modified tris-(2-(meth)acryloxyethyl)isocyanurate, are preferred, polyfunctional acrylate monomers that are trifunctional or higher and contain an isocyanurate structure in the molecule are more preferred, and ε-caprolactone-modified tris-(2-(meth)acryloxyethyl)isocyanurate is particularly preferred.These may be used alone or in combination of two or more. Furthermore, from the viewpoint of making it easier for the resulting adhesive to exhibit the desired viscoelasticity, the polyfunctional acrylate monomer preferably has a molecular weight of less than 20,000, more preferably less than 10,000, and particularly preferably less than 5,000. Furthermore, from the viewpoint of compatibility with the (meth)acrylic acid ester polymer (A), a polyfunctional acrylate monomer preferably has a molecular weight of less than 1,000.

[0079] When the adhesive composition P contains the active energy ray-curable component (D), the content of the active energy ray-curable component (D) is preferably 0.1 to 40 parts by mass, more preferably 1 to 30 parts by mass, particularly preferably 2 to 20 parts by mass, further preferably 3 to 15 parts by mass, and of these, preferably 4 to 10 parts by mass, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). This makes it easier to obtain better weather resistance.

[0080] (1-5) Photopolymerization initiator (E) When the adhesive composition P contains an active energy ray-curable component (D) and ultraviolet light is used as the active energy ray, the adhesive composition P preferably contains a photopolymerization initiator (E). By containing the photopolymerization initiator (E), the active energy ray-curable component (D) can be cured efficiently, and the polymerization curing time and the ultraviolet light irradiation dose can be reduced.

[0081] Examples of the photopolymerization initiator (E) include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin-n-butyl ether, benzoin isobutyl ether, acetophenone, dimethylaminoacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one, 4-(2-hydroxyethoxy)phenyl-2-(hydroxy-2-propyl)ketone, benzophenone, p-phenylbenzophenone, 4,4 Examples of suitable benzoxanthraquinones include 2-methyl-2-hydroxybenzoyl-1-methyl-1-methyl-2-methyl-1 ...

[0082] Among the above, from the viewpoint of suppressing the occurrence of needle-like cracks, phosphine-based photopolymerization initiators such as 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, or a mixture of 1-hydroxycyclohexyl phenyl ketone and benzophenone are preferred, and 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide is particularly preferred.

[0083] The content of the photopolymerization initiator (E) in the adhesive composition P is preferably 1 to 30 parts by mass, particularly preferably 5 to 25 parts by mass, and even more preferably 10 to 20 parts by mass, per 100 parts by mass of the active energy ray-curable component (D), which makes it easier for the resulting adhesive to satisfy the physical properties described below.

[0084] (1-6) Silane Coupling Agent (F) The adhesive composition P preferably further contains a silane coupling agent (F). This improves the adhesion of the resulting adhesive to a glass member when the adherend is a glass member. Furthermore, even when the adherend is a plastic plate, the resulting adhesive improves the adhesion to the plastic plate. This makes it easier to obtain better weather resistance.

[0085] The silane coupling agent (F) is preferably an organosilicon compound having at least one alkoxysilyl group in the molecule, which has good compatibility with the (meth)acrylic acid ester polymer (A) and has optical transparency.

[0086] Examples of such silane coupling agents (F) include polymerizable unsaturated group-containing silicon compounds such as vinyltrimethoxysilane, vinyltriethoxysilane, and methacryloxypropyltrimethoxysilane; silicon compounds having an epoxy structure such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, and 3-mercaptopropyldimethoxymethylsilane; Examples of suitable silicon compounds include hydroxyl group-containing silicon compounds, amino group-containing silicon compounds such as 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane, and 3-isocyanatepropyltriethoxysilane, as well as condensates of at least one of these with alkyl group-containing silicon compounds such as methyltriethoxysilane, ethyltriethoxysilane, methyltrimethoxysilane, and ethyltrimethoxysilane. These may be used alone or in combination of two or more.

[0087] The content of the silane coupling agent (F) in the adhesive composition P is preferably 0.01 to 10 parts by mass, more preferably 0.04 to 5 parts by mass, particularly preferably 0.08 to 1 part by mass, even more preferably 0.12 to 0.7 parts by mass, and of these, preferably 0.15 to 0.4 parts by mass, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). This allows the resulting adhesive to exhibit excellent adhesion and to have even better weather resistance and blister resistance.

[0088] (1-7) Ultraviolet absorber (G) The adhesive composition P preferably further contains an ultraviolet absorber (G), which allows the resulting adhesive to more effectively suppress the occurrence of needle-like cracks and has better weather resistance.

[0089] Examples of the ultraviolet absorber (G) include compounds such as benzophenones, benzotriazoles, benzoates, benzoxazinones, triazines, phenyl salicylates, cyanoacrylates, and nickel complex salts. Among these, benzophenones or triazines are preferred from the viewpoints of the effect of suppressing needle cracks and compatibility with the (meth)acrylic acid ester polymer (A). These may be used alone or in combination of two or more.

[0090] Examples of the benzophenone compounds include 2,2-dihydroxy-4-methoxybenzophenone, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid hydrate, and 2-hydroxy-4-n-octyloxybenzophenone.

[0091] Examples of the triazine compounds include 2,4-bis[2-hydroxy-4-butoxyphenyl]-6-(2,4-dibutoxyphenyl)-1,3-5-triazine, 2-[4,6-di(2,4-xylyl)-1,3,5-triazin-2-yl]-5-octyloxyphenol, and 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl]-5-[3-(dodecyloxy)-2-hydroxypropoxy]phenol.

[0092] When the adhesive composition P contains an ultraviolet absorber (G), the content of the ultraviolet absorber (G) is preferably 0.01 to 10 parts by mass, more preferably 0.04 to 5 parts by mass, particularly preferably 0.08 to 1 part by mass, even more preferably 0.1 to 0.7 parts by mass, and of these, preferably 0.2 to 0.5 parts by mass, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). This makes it easier for the adhesive composition P to satisfy the physical properties described below, and results in more excellent weather resistance and blister resistance.

[0093] (1-8) Light Stabilizer (H) The adhesive composition P preferably further contains a light stabilizer (H), which makes it possible to more effectively suppress the occurrence of needle-like cracks in the resulting adhesive and provides it with superior weather resistance.

[0094] Examples of the light stabilizer (H) include hindered amine and hindered phenol light stabilizers, among which hindered amine light stabilizers (HALS) are preferred because they provide the above-mentioned effects more effectively. Examples of the hindered amine light stabilizer include N-CH 3 Examples of such HALS include N-type HALS, N-H type HALS, NO-alkyl type HALS, reactive type HALS having a (meth)acrylic group, and high molecular weight type HALS. Of these, NO-alkyl type HALS are preferred because they provide the above-mentioned effects more effectively. A preferred example of an NO-alkyl type HALS is bis(1-undecanoxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate. These may be used alone or in combination of two or more.

[0095] When the adhesive composition P contains a light stabilizer (H), the content of the light stabilizer (H) is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 7 parts by mass, particularly preferably 0.1 to 5 parts by mass, even more preferably 0.4 to 3 parts by mass, and of these, preferably 0.8 to 2 parts by mass, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). This makes it easier for the adhesive composition P to satisfy the physical properties described below, and results in more excellent weather resistance.

[0096] (1-9) Antioxidant (I) The adhesive composition P preferably further contains an antioxidant (I), which allows the resulting adhesive to more effectively suppress the occurrence of needle-like cracks and has better weather resistance.

[0097] Examples of the antioxidant (I) include hindered phenol compounds such as triethylene glycol bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], pentaerythrityl tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,2-thio-diethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], n-octadecyl-3-(4'-hydroxy-3',5'-di-t-butylphenyl)propionate, and octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate; tris(2,4 Examples of suitable antioxidants include phosphorous ester compounds such as 2,2-methylenebis(4,6-di-t-butylphenyl) octyl phosphite, bis(2,6-di-t-butylphenyl)pentaerythritol diphosphite, and tetrakis(2,4-di-t-butylphenyl)4,4'-biphenylene diphosphonite; and sulfur-based antioxidants such as 2-mercaptobenzimidazole, pentaerythritol tetrakis(3-laurylthiopropionate), bis(dibutyldithiocarbamate)nickel(II), nickel diethyldithiocarbamate, and 3,3'-dilauryl thiodipropionate. Among these, hindered phenol compounds are preferred, as they provide the above-mentioned effects more effectively, and octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate is particularly preferred. These antioxidants may be used alone or in combination of two or more.

[0098] When the adhesive composition P contains the antioxidant (I), the content of the antioxidant (I) is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 7 parts by mass, particularly preferably 0.1 to 5 parts by mass, even more preferably 0.4 to 3 parts by mass, and especially preferably 0.8 to 2 parts by mass, relative to 100 parts by mass of the (meth)acrylic acid ester polymer (A). This makes it easier for the adhesive composition P to satisfy the physical properties described below and provides better weather resistance.

[0099] (1-10) Various Additives The adhesive composition P may contain, if desired, various additives that are commonly used in acrylic adhesives, such as antistatic agents, tackifiers, colorants, infrared absorbers, rust inhibitors, softeners, fillers, plasticizers, and refractive index adjusters.

[0100] (2) Production of Adhesive Composition The adhesive composition P can be produced by producing a (meth)acrylic acid ester polymer (A), mixing the obtained (meth)acrylic acid ester polymer (A) with a crosslinking agent (B) and an oxygen absorber (C), and, if desired, adding an active energy ray-curable component (D), a photopolymerization initiator (E), a silane coupling agent (F), an ultraviolet absorber (G), a light stabilizer (H), an antioxidant (I), an additive, etc.

[0101] The (meth)acrylic acid ester polymer (A) can be produced by polymerizing a mixture of monomers constituting the polymer by a conventional radical polymerization method. The polymerization of the (meth)acrylic acid ester polymer (A) is preferably carried out by a solution polymerization method using a polymerization initiator as desired. However, the present invention is not limited thereto, and the polymerization may be carried out in the absence of a solvent.

[0102] Examples of polymerization solvents include ethyl acetate, n-butyl acetate, isobutyl acetate, toluene, acetone, hexane, and methyl ethyl ketone, and two or more of these may be used in combination. Examples of polymerization initiators include azo compounds and organic peroxides, and two or more of these may be used in combination. In the polymerization step, the weight-average molecular weight of the resulting polymer can be adjusted by adding a chain transfer agent such as 2-mercaptoethanol.

[0103] Once the (meth)acrylic acid ester polymer (A) is obtained, a crosslinking agent (B), an oxygen absorber (C), and optionally an active energy ray-curable component (D), a photopolymerization initiator (E), a silane coupling agent (F), an ultraviolet absorber (G), a light stabilizer (H), an antioxidant (I), additives, a dilution solvent, etc. are added to a solution of the (meth)acrylic acid ester polymer (A) and thoroughly mixed to obtain an adhesive composition P (coating solution) diluted with a solvent. Note that when any of the above components is used in a solid state or when precipitation occurs when mixed with other components in an undiluted state, that component may be dissolved or diluted alone in a dilution solvent before being mixed with the other components.

[0104] Examples of the dilution solvent include aliphatic hydrocarbons such as hexane, heptane, and cyclohexane; aromatic hydrocarbons such as toluene and xylene; halogenated hydrocarbons such as methylene chloride and ethylene chloride; alcohols such as methanol, ethanol, propanol, butanol, and 1-methoxy-2-propanol; ketones such as acetone, methyl ethyl ketone, 2-pentanone, isophorone, and cyclohexanone; esters such as ethyl acetate and butyl acetate; and cellosolve-based solvents such as ethyl cellosolve.

[0105] The concentration and viscosity of the coating solution prepared in this manner are not particularly limited as long as they are within a range that allows coating, and can be appropriately selected depending on the situation. For example, the adhesive composition P is diluted so that the concentration is 10 to 60 mass %. Note that the addition of a dilution solvent or the like is not a necessary condition for obtaining the coating solution, and as long as the adhesive composition P has a viscosity that allows coating, the addition of a dilution solvent is not necessary. In this case, the adhesive composition P becomes a coating solution in which the polymerization solvent for the (meth)acrylic acid ester polymer (A) is used as the dilution solvent.

[0106] (3) Production of Adhesive The adhesive composition P described above is applied to a desired object and then crosslinked to obtain an adhesive (adhesive layer).

[0107] The adhesive composition P can be crosslinked by a heat treatment. This heat treatment can also serve as a drying treatment after application of the adhesive composition P. The heating temperature for the heat treatment is preferably 50 to 150°C, and more preferably 70 to 120°C. The heating time is preferably 10 seconds to 10 minutes, and more preferably 50 seconds to 2 minutes.

[0108] After the heat treatment, a curing period of about 1 to 2 weeks may be provided at room temperature (e.g., 23°C, 50% RH), if necessary. If this curing period is required, the adhesive is formed after the curing period has elapsed; if no curing period is required, the adhesive is formed after the heat treatment has been completed. In this specification, "relative humidity α%" may also be expressed as "α% RH" (RH; Relative humidity).

[0109] By the above heat treatment (and curing), a crosslinked product of the (meth)acrylic acid ester polymer (A) crosslinked by the crosslinking agent (B) is formed.

[0110] (4) Physical Properties (Gel Fraction) The gel fraction of the adhesive according to this embodiment is preferably 20 to 85%, more preferably 30 to 70%, particularly preferably 40 to 60%, even more preferably 45 to 55%, and most preferably 47 to 50%. This makes it easier to obtain good pressure-sensitive adhesive properties when applied to an adherend. The method for measuring the gel fraction in this specification is as shown in the test examples described below.

[0111] When the adhesive according to this embodiment is active energy ray-curable, the gel fraction of the adhesive after active energy ray curing is preferably 30 to 99%, more preferably 40 to 90%, particularly preferably 45 to 80%, even more preferably 50 to 74%, and of these, preferably 55 to 68%, most preferably 60 to 63%. This tends to result in good adhesive strength after attachment to an adherend.

[0112] [Adhesive Sheet] The adhesive sheet according to this embodiment has an adhesive layer for bonding two members together. At least one of the members is an optical member. The specific configuration of the adhesive sheet and the optical member will be described later.

[0113] The adhesive layer in the adhesive sheet according to this embodiment is made of the adhesive according to the embodiment described above.

[0114] The thickness of the adhesive layer of the adhesive sheet according to this embodiment (measured in accordance with JIS K7130) is preferably 1 to 1000 μm, more preferably 10 to 800 μm, and particularly preferably 30 to 600 μm, from the viewpoint of adhesive strength and weather resistance; and from the viewpoint of weather resistance, it is preferably 50 to 400 μm, even more preferably 80 to 300 μm, and of these, it is preferably 120 to 260 μm.

[0115] (1) Physical Properties (1-1) Gel Fraction / Gel Fraction Change Rate In the adhesive sheet according to this embodiment, the adhesive layer after laminating two members was subjected to an illuminance of 100 mW / cm 2 After 120 hours of irradiation with ultraviolet light (hereinafter sometimes referred to as "S-UV irradiation"), the gel fraction of the adhesive constituting the adhesive layer is preferably 40 to 99%, more preferably 50 to 95%, particularly preferably 55 to 90%, even more preferably 60 to 85%, and of these, preferably 65 to 80%. This allows the adhesive to exert a predetermined cohesive force even after S-UV irradiation, making it easier to obtain excellent weather resistance.

[0116] Here, in this specification, "adhesive layer after lamination" means an adhesive layer in the same state as the adhesive layer of the adhesive sheet if the adhesive layer is not active energy ray-curable, and means an adhesive layer cured by active energy ray irradiation after lamination if the adhesive layer is active energy ray-curable. "Adhesive layer after active energy ray curing" means an adhesive layer that has been completely cured by active energy ray irradiation. Specifically, this refers to an adhesive layer in which the rate of increase in gel fraction of the adhesive layer is 10% or less when the active energy ray-cured adhesive layer is further irradiated with active energy ray at the same dose (light amount) as when the active energy ray cured adhesive layer was cured with the active energy ray, and particularly refers to an adhesive layer in which the rate of increase is 5% or less.

[0117] In the adhesive sheet according to this embodiment, when the gel fraction of the adhesive constituting the adhesive layer after lamination is defined as G1, and the gel fraction of the adhesive constituting the adhesive layer after lamination and S-UV irradiation is defined as G2, the gel fraction change rate ((G2 / G1) x 100) (%), which is the ratio of G2 to G1, is preferably 120% or less, more preferably 117% or less, particularly preferably 115% or less, even more preferably 112% or less, and of these, preferably 109% or less. This suppresses the destruction of crosslinking points that could serve as starting points for needle-like cracks, and exhibits good lamination properties to the adherend. In other words, the occurrence of needle-like cracks can be more effectively suppressed, resulting in better weather resistance.

[0118] The lower limit of the gel fraction change rate is not particularly limited, but is preferably 100% or more, more preferably 103% or more, and even more preferably 105% or more.

[0119] (1-2) Average Peak Molecular Weight of Sol Content In this embodiment, the average peak molecular weight of the sol content of the adhesive constituting the adhesive layer after lamination is preferably 10,000 to 250,000, more preferably 30,000 to 200,000, particularly preferably 40,000 to 150,000, even more preferably 50,000 to 100,000, and most preferably 60,000 to 80,000. This makes it easier to achieve good adhesive strength after lamination of the components. Note that the average peak molecular weight of the sol content in this specification is a value measured by gel permeation chromatography (GPC) in terms of standard polystyrene. Specific measurement methods are as shown in the test examples described below.

[0120] The average peak molecular weight of the sol component of the adhesive after S-UV irradiation of the adhesive layer after lamination (hereinafter simply referred to as "adhesive after S-UV irradiation") is preferably 10,000 to 200,000, more preferably 20,000 to 150,000, particularly preferably 30,000 to 100,000, even more preferably 40,000 to 70,000, and of these, preferably 50,000 to 58,000. This makes it possible to more effectively suppress the occurrence of needle-like cracks, resulting in better weather resistance.

[0121] (1-3) Storage Modulus G' In this embodiment, the storage modulus G' at 23°C of the adhesive constituting the adhesive layer after lamination is preferably 0.001 to 2 MPa, more preferably 0.005 to 1 MPa, more preferably 0.01 to 0.5 MPa, particularly preferably 0.02 to 0.1 MPa, and even more preferably 0.03 to 0.07 MPa. This makes it easier to achieve good adhesive strength after lamination of the members. The method for measuring the storage modulus G' in this specification is as shown in the test examples described below.

[0122] The storage modulus G' of the adhesive at 23°C after S-UV irradiation is preferably 0.0001 to 2 MPa, preferably 0.005 to 1 MPa, more preferably 0.01 to 0.5 MPa, particularly preferably 0.03 to 0.2 MPa, even more preferably 0.05 to 0.15 MPa, and of these, preferably 0.07 to 0.1 MPa. This makes it possible to more effectively suppress the occurrence of needle-like cracks, resulting in better weather resistance.

[0123] The storage modulus G' at -15°C of the adhesive constituting the adhesive layer after lamination is preferably 0.01 to 100 MPa, more preferably 0.1 to 50 MPa, more preferably 1 to 25 MPa, particularly preferably 2 to 10 MPa, and even more preferably 3.0 to 5.0 MPa. This makes it easier to achieve good adhesive strength at low temperatures after lamination of the members.

[0124] The storage modulus G' of the adhesive at -15°C after S-UV irradiation is preferably 0.01 to 100 MPa, more preferably 0.1 to 50 MPa, more preferably 1 to 25 MPa, particularly preferably 3 to 10.0 MPa, and even more preferably 6 to 9.5 MPa. This makes it possible to more effectively suppress the occurrence of needle-like cracks, resulting in better weather resistance.

[0125] The storage modulus G' at 100°C of the adhesive constituting the adhesive layer after lamination is preferably 0.0001 to 2 MPa, more preferably 0.0005 to 1 MPa, more preferably 0.001 to 0.1 MPa, particularly preferably 0.003 to 0.05 MPa, even more preferably 0.005 to 0.02 MPa, and of these, preferably 0.007 to 0.012 MPa. This makes it easier to achieve good adhesive strength at high temperatures after lamination of the members.

[0126] The storage modulus G' of the adhesive at 100°C after S-UV irradiation is preferably 0.0001 to 2 MPa, more preferably 0.0005 to 1 MPa, more preferably 0.001 to 0.1 MPa, particularly preferably 0.002 to 0.05 MPa, even more preferably 0.003 to 0.02 MPa, and of these, preferably 0.004 to 0.01 MPa. This makes it possible to more effectively suppress the occurrence of needle-like cracks, resulting in better weather resistance.

[0127] (1-4) Peak Temperature of Loss Tangent tanδ The peak temperature Tb of the loss tangent tanδ of the adhesive constituting the adhesive layer after lamination is preferably −40 to 20°C, more preferably −30 to 10°C, particularly preferably −25 to 0°C, further preferably −20 to −5°C, and of these, preferably −15 to −10°C. This makes it easier to obtain good adhesive strength after lamination of the members. The method for measuring the loss tangent tanδ is as shown in the test examples described below.

[0128] The peak temperature Ta of the loss tangent tanδ of the adhesive after S-UV irradiation is preferably −40 to 20° C., more preferably −30 to 10° C., particularly preferably −24 to 5° C., further preferably −18 to 0° C., and of these, preferably −12 to −7° C. This makes it possible to more effectively suppress the occurrence of needle-like cracks, resulting in better weather resistance.

[0129] The value obtained by subtracting Tb from Ta (Ta - Tb) is preferably 0 to 30, more preferably 0.1 to 20, particularly preferably 0.4 to 10, even more preferably 0.8 to 5, and most preferably 1 to 2. This shifts the peak temperature of the loss tangent tanδ to a higher temperature after S-UV irradiation, thereby tending to shift the point at which the adhesive's viscoelastic viscosity increases from the low temperature side to the room temperature side. As a result, destruction of crosslinking points that could serve as the starting point for needle-like cracks is suppressed, resulting in excellent adhesion to the adherend. In other words, the occurrence of needle-like cracks can be more effectively suppressed, resulting in better weather resistance.

[0130] (1-5) Adhesion Strength The adhesion strength of the adhesive layer of the adhesive sheet according to this embodiment to soda-lime glass after application is preferably 1 to 100 N / 25 mm, more preferably 10 to 90 N / 25 mm, particularly preferably 20 to 80 N / 25 mm, even more preferably 30 to 70 N / 25 mm, and most preferably 40 to 60 N / 25 mm. This tends to result in excellent weather resistance and blister resistance. The above-mentioned adhesion strength basically refers to the adhesion strength measured using the 180-degree peel method in accordance with JIS Z0237:2009, and the specific test method is as shown in the test examples described below.

[0131] (1-6) Total Light Transmittance The total light transmittance of the adhesive layer after lamination in the adhesive sheet according to this embodiment is preferably 80% or more, more preferably 90% or more, particularly preferably 95% or more, and even more preferably 99% or more. This provides very high transparency and makes the sheet suitable for optical applications (displays). The upper limit of the total light transmittance is not particularly limited, and may be 100%, or may be a value slightly exceeding 100% due to measurement considerations. The total light transmittance of the adhesive layer after S-UV irradiation is also preferably in the same numerical range as above. The total light transmittance in this specification is a value measured in accordance with JIS K7361-1:1997, and specific test methods are as shown in the test examples described below.

[0132] (1-7) Haze Value The haze value of the adhesive layer after lamination in the adhesive sheet according to this embodiment is preferably 2% or less, and particularly preferably 1% or less. This provides very high transparency and makes it suitable for optical applications (for displays). The lower limit of the haze value is not particularly restricted and may be 0%. The haze value of the adhesive layer after S-UV irradiation is also preferably in the same numerical range as above. The haze value in this specification is a value measured in accordance with JIS K7136:2000, and the specific test method is as shown in the test examples described below.

[0133] (1-8) Chromaticity b* The chromaticity b* (chromaticity b*1) of the adhesive layer after lamination in the adhesive sheet according to this embodiment, as defined by the CIE 1976 L*a*b* color system, is preferably -20 to 20, more preferably -10 to 10, particularly preferably -5 to 5, even more preferably -2 to 2, and most preferably -1 to 1, and most preferably -0.5 to 0.5. This makes the adhesive layer nearly colorless and transparent, making it suitable for optical applications.

[0134] The chromaticity b* (chromaticity b*2) of the adhesive layer after lamination and S-UV irradiation, as defined by the CIE 1976 L*a*b* color system, is preferably -20 to 20, more preferably -10 to 10, particularly preferably -5 to 5, even more preferably -3 to 3, and of these, preferably -1.2 to 1.2. This means that the adhesive layer has a small degree of yellowness even after S-UV irradiation, and can be said to have excellent weather resistance from the standpoint of chromaticity.

[0135] The absolute value of the ratio (b*2 / b*1) of the chromaticity b*2 to the chromaticity b*1 is preferably 10 or less, more preferably 6 or less, particularly preferably 3 or less, and even more preferably 2.5 or less. This reduces the degree of yellowing of the adhesive layer even after S-UV irradiation, and can be said to have excellent weather resistance from the standpoint of chromaticity. The lower limit of the absolute value of the ratio (b*2 / b*1) is not particularly limited, but is most preferably 1.

[0136] (2) Specific Configuration of Adhesive Sheet A specific configuration of one example of the adhesive sheet according to this embodiment is shown in Figure 1. As shown in Figure 1, adhesive sheet 1 according to one embodiment is composed of two release sheets 12a, 12b and adhesive layer 11 sandwiched between these two release sheets 12a, 12b so as to contact the release surfaces of these two release sheets 12a, 12b. Note that in this specification, the release surface of a release sheet refers to the surface of the release sheet that has releasability, and includes both a surface that has been subjected to a release treatment and a surface that exhibits releasability even without being subjected to a release treatment.

[0137] The adhesive layer 11 is made of the adhesive according to the embodiment described above. The release sheets 12a and 12b protect the adhesive layer until the adhesive sheet is in use, and are peeled off when the adhesive sheet (adhesive layer) is to be used. In the adhesive sheet 1 according to this embodiment, one or both of the release sheets 12a and 12b are not necessarily required.

[0138] Examples of materials that can be used as the release sheets 12a and 12b include polyethylene films, polypropylene films, polybutene films, polybutadiene films, polymethylpentene films, polyvinyl chloride films, vinyl chloride copolymer films, polyethylene terephthalate films, polyethylene naphthalate films, polybutylene terephthalate films, polyurethane films, ethylene vinyl acetate films, ionomer resin films, ethylene-(meth)acrylic acid copolymer films, ethylene-(meth)acrylic acid ester polymer films, polystyrene films, polycarbonate films, polyimide films, and fluororesin films. Crosslinked films of these materials can also be used. Furthermore, laminated films of these materials may also be used. From the perspective of the SDGs, the material constituting the release sheets may be a material with a high biomass content, a recyclable or reusable material, or a recycled or reused material.

[0139] It is preferable that the release surfaces of the release sheets 12a and 12b (particularly the surfaces that come into contact with the adhesive layer 11) are subjected to a release treatment. Examples of release agents used for the release treatment include alkyd-based, silicone-based, fluorine-based, unsaturated polyester-based, polyolefin-based, and wax-based release agents.

[0140] There is no particular limitation on the thickness of the release sheets 12a and 12b, but it is usually about 20 to 150 μm.

[0141] From the viewpoint of ease of handling, it is preferable that one of the two release sheets 12a, 12b be a heavy release type release sheet with a high release strength and the other be a light release type release sheet with a low release strength.

[0142] (3) Manufacturing of Adhesive Sheet In one manufacturing example of adhesive sheet 1, a coating solution of the adhesive composition P is applied to the release surface of one release sheet 12a (or 12b), and a heat treatment is carried out to thermally crosslink the adhesive composition P to form a coating layer, after which the release surface of the other release sheet 12b (or 12a) is superimposed on the coating layer. If a curing period is required, a curing period is allowed, but if no curing period is required, the coating layer becomes adhesive layer 11 as is. Through the above steps, adhesive sheet 1 is obtained. The conditions for the heat treatment and curing are as described above.

[0143] The adhesive composition P can be applied by a coating solution such as bar coating, knife coating, roll coating, blade coating, die coating, or gravure coating.

[0144] (4) Use The adhesive sheet according to this embodiment is used to bond two members together, at least one of which is an optical member.

[0145] Examples of optical components include components constituting a display body (display body components) described below, as well as components constituting a solar cell, and components constituting a mobile body (car, ship, aircraft, etc.) or building (windows, exterior materials, interior materials, etc.), and are usually components made of a light-transmitting plastic plate, plastic film, glass plate, glass film, etc., or components containing any of these.

[0146] The other of the two members may be an optical member or a member made of an opaque or translucent material, such as metal, ceramics, colored plastic, colored glass, graphite, paper, wood, stone, mortar, plaster, or the like, or a member containing any of these.

[0147] [Optical Construction] An optical construction according to one embodiment of the present invention is formed by bonding at least two members together with an adhesive layer, at least one of which is an optical member. The adhesive layer is formed from the adhesive according to the above-described embodiment, or from the adhesive layer of the adhesive sheet according to the above-described embodiment.

[0148] The thickness of the adhesive layer in this embodiment is the same as that of the adhesive layer of the adhesive sheet according to the above-described embodiment, and the optical member is as described in the above-described embodiment.

[0149] To manufacture the optical construction according to this embodiment, for example, the adhesive coating liquid described above is applied to one component to form an adhesive layer, and then another component is bonded to the adhesive layer. As another example, the adhesive layer of the adhesive sheet described above is bonded to one component, and then another component is bonded to the adhesive layer.

[0150] Here, when the adhesive layer is active energy ray-curable, it is preferable to cure the adhesive layer by irradiating it with active energy rays through any member (member that transmits active energy rays) after the lamination.

[0151] The active energy ray refers to an electromagnetic wave or a charged particle beam that has an energy quantum, and specific examples thereof include ultraviolet rays, electron beams, etc. Among active energy rays, ultraviolet rays are particularly preferred because they are easy to handle.

[0152] The ultraviolet irradiation can be performed using a high-pressure mercury lamp, a Heraeus H lamp, a xenon lamp, or the like, and the amount of ultraviolet irradiation is set to an illuminance of 50 to 1000 mW / cm. 2 The light intensity is preferably about 50 to 10,000 mJ / cm. 2 is preferably 80 to 5000 mJ / cm 2 More preferably, it is 300 to 2000 mJ / cm 2 On the other hand, the electron beam irradiation can be carried out by an electron beam accelerator or the like, and the irradiation dose of the electron beam is preferably about 10 to 1000 krad.

[0153] [Display Body] A display body according to one embodiment of the present invention includes one display body component, another display body component, and an adhesive layer that bonds the one display body component and the other display body component to each other. The adhesive layer is formed from the adhesive layer of the adhesive sheet according to the embodiment described above.

[0154] At least one of the one display member constituting member and the other display member constituting member may have a step at least on the surface on the side to be bonded by the adhesive layer.

[0155] Both the first display member and the second display member may be hard plates. When two hard plates are bonded together, the hard plates are rigid and inflexible, so that the adhesive layer is attached to one of the hard plates and the two hard plates are pressed vertically to bring the hard plates into close contact with the adhesive layer, thereby bonding the two hard plates together.

[0156] A display according to one embodiment of the present invention will be described with reference to the drawings. As shown in Fig. 2, the display 2 according to this embodiment is configured to include a first display component 21 (one display component), a second display component 22 (another display component), and an adhesive layer 11 located therebetween that bonds the first display component 21 and the second display component 22 to each other.

[0157] At least one of the first display body component 21 and the second display body component 22 may have a step on the surface that is bonded to the first display body component 21 by the adhesive layer 11. In the present embodiment shown in Fig. 2, the first display body component 21 has a step on the surface on the adhesive layer 11 side due to the printing layer 3 or the like.

[0158] The adhesive layer 11 in the display body 2 is either the adhesive layer 11 (non-curable by active energy rays) of the adhesive sheet 1 described above, or the adhesive layer 11 (curable by active energy rays) of the adhesive sheet 1 described above that has been cured by irradiation with active energy rays.

[0159] Examples of the display 2 include a liquid crystal (LCD) display, a light-emitting diode (LED) display, an organic electroluminescence (OLED) display, and electronic paper, and may also be a touch panel. Note that LED displays also include those using mini LEDs and micro LEDs.

[0160] The first display member 21 is preferably a protective panel made of a glass plate, a plastic plate, or a laminate containing these. In this case, the printing layer 3 is generally formed in a frame shape on the adhesive layer 11 side of the first display member 21.

[0161] The glass plate is not particularly limited, and examples thereof include chemically strengthened glass, alkali-free glass, quartz glass, soda-lime glass, barium-strontium-containing glass, aluminosilicate glass, lead glass, borosilicate glass, barium borosilicate glass, etc. The thickness of the glass plate is not particularly limited, but is usually 0.1 to 5 mm, and preferably 0.2 to 2 mm.

[0162] The plastic plate is not particularly limited, and examples thereof include an acrylic plate, a polycarbonate plate, etc. The thickness of the plastic plate is not particularly limited, but is usually 0.2 to 5 mm, and preferably 0.4 to 3 mm.

[0163] On one or both sides of the glass plate or plastic plate, various functional layers (transparent conductive film, metal layer, silica layer, hard coat layer, anti-glare layer, etc.) may be provided, or optical members may be laminated. Furthermore, the transparent conductive film and metal layer may be patterned.

[0164] The second display component 22 is preferably an optical element to be attached to the first display component 21, a display module (e.g., a liquid crystal (LCD) module, a light-emitting diode (LED) module, an organic electroluminescence (organic EL) module, etc.), an optical element as part of a display module, or a laminate including a display module.

[0165] Examples of the optical member include a shatterproof film, a polarizing plate (polarizing film), a polarizer, a retardation plate (retardation film), a viewing angle compensation film, a brightness improvement film, a contrast improvement film, a liquid crystal polymer film, a diffusion film, a semi-transmitting reflective film, a transparent conductive film, etc. A preferred example of the transparent conductive film is an ITO-PET film in which a tin-doped indium oxide (ITO) layer is formed on one surface of a polyethylene terephthalate film.

[0166] The material constituting the printing layer 3 is not particularly limited, and known materials for printing can be used. The thickness of the printing layer 3, i.e., the height of the step, is preferably 0.5 to 50 μm, more preferably 1 to 30 μm, and particularly preferably 3 to 20 μm. When the thickness of the printing layer 3 is within the above range, the step-following ability of the adhesive layer 11 is effectively exhibited, and the concealing property that is the purpose of the printing layer 3 can be sufficiently ensured. Note that the printing layer 3 is generally formed in a frame shape on the adhesive layer 11 side of the display component.

[0167] To manufacture the display body 2, as an example, one of the release sheets 12a of the adhesive sheet 1 is peeled off, and the exposed adhesive layer 11 of the adhesive sheet 1 is attached to the surface of the first display body component 21 on which the printing layer 3 is present.

[0168] Next, the other release sheet 12b is peeled off from the adhesive layer 11 of the adhesive sheet 1, and the exposed adhesive layer 11 of the adhesive sheet 1 is bonded to the second display body component 22 to obtain the display body. As another example, the bonding order of the first display body component 21 and the second display body component 22 may be reversed.

[0169] Here, when the adhesive layer 11 is active energy ray curable (when it contains an active energy ray curable component (D)), after bonding the laminate of the first display body component 21 and the adhesive layer 11 to the second display body component 22, it is preferable to irradiate the adhesive layer 11 with active energy rays through the first display body component 21 and / or the second display body component 22 to cure the adhesive layer 11.

[0170] In the display body 2, the adhesive constituting the adhesive layer 11 contains the oxygen absorber described above, so even when exposed to high-intensity ultraviolet light for a long period of time (for example, 20 hours, 40 hours, 80 hours, or in some cases 120 hours), the occurrence of needle-like cracks in the adhesive layer 11 is suppressed, resulting in excellent weather resistance.

[0171] The above-described embodiments have been described to facilitate understanding of the present invention, and are not intended to limit the present invention. Therefore, each element disclosed in the above embodiments is intended to include all design modifications and equivalents that fall within the technical scope of the present invention.

[0172] For example, one or both of the release sheets 12a and 12b in the adhesive sheet 1 may be omitted, or a desired optical member may be laminated in place of the release sheets 12a and / or 12b. The first display body component 21 may not have a step. Furthermore, not only the first display body component 21 but also the second display body component 22 may have a step on the adhesive layer 11 side.

[0173] In this specification, when it is stated that "X to Y" (X and Y are any numbers), it means "X or more and Y or less" unless otherwise specified, and also means "preferably greater than X" or "preferably smaller than Y". Furthermore, when it is stated that "X or more" (X is any number), it means "preferably greater than X" unless otherwise specified, and when it is stated that "Y or less" (Y is any number), it also means "preferably smaller than Y" unless otherwise specified.

[0174] The present invention will be explained in more detail below with reference to examples, but the scope of the present invention is not limited to these examples.

[0175] Example 1 1. Preparation of (meth)acrylic acid ester polymer 65 parts by mass of 2-ethylhexyl acrylate, 15 parts by mass of isobornyl acrylate, 5 parts by mass of N-acryloylmorpholine, and 15 parts by mass of 2-hydroxyethyl acrylate were copolymerized by solution polymerization to prepare a (meth)acrylic acid ester polymer (A). The molecular weight of this (meth)acrylic acid ester polymer (A) was measured by the method described below, and the weight average molecular weight (Mw) was found to be 500,000.

[0176] 2. Preparation of Adhesive Composition A mixture of 100 parts by mass (solid content equivalent; the same applies hereinafter) of the (meth)acrylic acid ester polymer (A) obtained in the above step 1, 0.17 parts by mass of an isocyanate-based crosslinking agent (manufactured by Mitsui Chemicals, Inc., product name "Takenate D-101E"), and a compound represented by the following formula (III) as an oxygen absorber (C) was prepared. (manufactured by Kuraray Co., Ltd., product name "Diprenyl Glycerin Ether (DPNG)")), 5.2 parts by mass of ε-caprolactone-modified tris-(2-acryloxyethyl)isocyanurate (manufactured by Shin-Nakamura Chemical Co., Ltd., product name "NK Ester A-9300-1CL") as the active energy ray-curable component (D), 0.92 parts by mass of 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide (E1) as the photopolymerization initiator (E), and 0.25 parts by mass of 3-glycidoxypropyltrimethoxysilane as the silane coupling agent (F) were mixed, thoroughly stirred, and diluted with methyl ethyl ketone to obtain a coating solution of an adhesive composition.

[0177] Here, the formulations (solid content equivalent) of the adhesive compositions when the (meth)acrylic acid ester polymer (A) is taken as 100 parts by mass (solid content equivalent) are shown in Table 1. The details of the abbreviations and the like shown in Table 1 are as follows: [(Meth)acrylic acid ester polymer (A)] 2EHA: 2-ethylhexyl acrylate IBXA: isobornyl acrylate ACMO: N-acryloylmorpholine HEA: 2-hydroxyethyl acrylate [Photopolymerization initiator (E)] E1: 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide E2: mixture of 1-hydroxycyclohexyl phenyl ketone and benzophenone (mass ratio 50:50) [Ultraviolet absorber (G)] G1: 2,2-dihydroxy-4-methoxybenzophenone G2: 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl]-5-[3-(dodecyloxy)-2-hydroxypropoxy]phenol

[0178] 3. Manufacturing of Adhesive Sheet The coating solution of the adhesive composition obtained in step 2 above was applied with a coater to the release-treated surface of a heavy-release type release sheet R1, which had been prepared by treating one side of a polyethylene terephthalate film with a silicone-based release agent. This was then heated at 90°C for 1 minute to form a coating layer. The coating layer on the release sheet R1 obtained above was then bonded to a light-release type release sheet R2, which had been prepared by treating one side of a polyethylene terephthalate film with a silicone-based release agent, so that the release-treated surface of the release sheet R2 was in contact with the coating layer. This was then aged for 7 days under conditions of 23°C and 50% RH to produce an adhesive sheet having a 50 μm-thick adhesive layer, i.e., an adhesive sheet having a configuration of release sheet R1 / adhesive layer (thickness: 50 μm) / release sheet R2.

[0179] The thickness of the adhesive layer was measured using a constant pressure thickness measuring device (manufactured by Teclock Corporation, product name "PG-02") in accordance with JIS K 7130. Furthermore, it was confirmed that the release strength of release sheet R1 was greater than that of release sheet R2 in the obtained adhesive sheet.

[0180] Examples 2 to 5, Comparative Examples 1 and 2 Adhesive sheets were produced in the same manner as in Example 1, except that the amount of oxygen absorber (C) and the type of photopolymerization initiator (E) were changed as shown in Table 1. In Examples 2 and 3, an ultraviolet absorber (G) (G1 / G2) was also added in the amount shown in Table 1. In Example 4, bis(1-undecanoxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate was also added as a light stabilizer (H) in the amount shown in Table 1. In Example 5, octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was also added as an antioxidant (I) in the amount shown in Table 1.

[0181] The weight average molecular weight (Mw) is a polystyrene-equivalent weight average molecular weight measured by gel permeation chromatography (GPC) under the following conditions (GPC measurement). <Measurement conditions> Measurement device: HLC-8320, manufactured by Tosoh Corporation GPC columns (passed in the following order): TSK gel super H-H, TSK gel super HM-H, TSK gel super H2000, manufactured by Tosoh Corporation Measurement solvent: tetrahydrofuran Measurement temperature: 40°C

[0182] [Test Example 1] (Measurement of gel fraction) A 250 μm thick adhesive layer was produced by laminating multiple adhesive layers of the adhesive sheets produced in the Examples and Comparative Examples. The adhesive layer (thickness: 250 μm) was cut to a size of 70 mm x 150 mm, and the adhesive layer was wrapped in a polyester mesh (mesh size 200). The mass was weighed using a precision balance, and the mass of the mesh alone was subtracted to calculate the mass of the adhesive alone. This mass was designated M1.

[0183] Next, the adhesive wrapped in the polyester mesh was immersed in ethyl acetate at room temperature (23°C) for 24 hours. The adhesive was then removed and air-dried for 24 hours in an environment at 23°C and 50% RH, and then dried in an oven at 80°C for 12 hours. After drying, the mass was weighed using a precision balance, and the mass of the adhesive alone was calculated by subtracting the mass of the mesh alone. This mass was designated M2. The gel fraction (%; G0) was expressed as (M2 / M1) x 100. The results are shown in Table 2.

[0184] In addition, a 250 μm thick adhesive layer was produced by laminating multiple adhesive layers of the adhesive sheets produced in the Examples and Comparative Examples. The adhesive layer (thickness: 250 μm) was irradiated with active energy rays (ultraviolet rays; UV) to cure the adhesive layer. The gel fraction (%; G1) of the adhesive in the adhesive layer after curing with active energy rays was measured in the same manner as above. The results are shown in Table 2. The irradiation conditions for active energy rays were as follows:

[0185] <Activated energy ray irradiation conditions> - High pressure mercury lamp used - Illuminance: 200 mW / cm 2 , Light amount: 1000mJ / cm 2 ・UV illuminance and light intensity meter used is "UVPF-A1" manufactured by iGraphics

[0186] Furthermore, a 250 μm thick adhesive layer was prepared by laminating multiple adhesive layers of the adhesive sheets produced in the Examples and Comparative Examples. This adhesive layer (thickness: 250 μm) was used to bond two soda-lime glass plates (manufactured by Nippon Sheet Glass Co., Ltd., thickness: 1.1 mm, length: 70 mm × width: 150 mm) to prepare a laminate (soda-lime glass plate / adhesive layer (250 μm) / soda-lime glass plate). The laminate was irradiated with active energy rays (ultraviolet rays; UV) under the active energy ray irradiation conditions described above to cure the adhesive layer. The resulting laminate was irradiated with ultraviolet rays (S-UV irradiation) under the following conditions. The adhesive layers of the laminate after S-UV irradiation were then separated from the two soda-lime glass plates. The gel fraction (%; G2) of the adhesive in the separated adhesive layer was measured in the same manner as described above. The results are shown in Table 2.

[0187] <Ultraviolet light irradiation conditions> Device: Eye Super UV Tester SUV-W151 (manufactured by Iwasaki Electric Co., Ltd.) UV lamp: ME06-L31WX / SUV (manufactured by Iwasaki Electric Co., Ltd.) Water-cooled jacket: WJ50-SUV-4 (manufactured by Iwasaki Electric Co., Ltd.) Illuminance: 100 mW / cm 2 Irradiation time: 120 hours Light intensity: 43.2 kJ / cm 2 Temperature: 63°C Humidity: 70% RH Temperature and humidity control: Closed circulation method

[0188] Based on the G1 and G2 obtained above, the gel fraction change rate ((G2 / G1)×100) (%), which is the ratio of G2 to G1, was calculated. The results are shown in Table 2.

[0189] [Test Example 2] (Measurement of the Average Peak Molecular Weight of the Sol Fraction) A 250 μm thick adhesive layer was prepared by laminating multiple adhesive layers from the adhesive sheets produced in the Examples and Comparative Examples. The adhesive layer (250 μm) was irradiated with active energy rays (ultraviolet rays; UV) under the same active energy ray irradiation conditions as in Test Example 1, thereby curing the adhesive layer. Ethyl acetate (after immersion in the adhesive and removal) obtained from the adhesive layer (250 μm) after active energy ray curing in the same manner as in Test Example 1 was concentrated in an evaporator to obtain a sol fraction. The sol fraction was then diluted with tetrahydrofuran to a 0.3% by mass solution, filtered through a 0.45 μm filter, and the average peak molecular weight (Mp; before S-UV) of the sol fraction was measured by GPC measurement. The measurement conditions for the GPC measurement were as described above. The results are shown in Table 2.

[0190] Additionally, a 250 μm thick adhesive layer was produced by laminating multiple adhesive layers from the adhesive sheets produced in the Examples and Comparative Examples. A laminate was produced using this adhesive layer (thickness: 250 μm) in the same manner as in Test Example 1. The laminate was irradiated with active energy rays (ultraviolet rays; UV) under the same active energy ray irradiation conditions as in Test Example 1 to cure the adhesive layer. The resulting laminate was irradiated with ultraviolet rays (S-UV irradiation). Then, for the laminate after S-UV irradiation, the adhesive layer was separated from the two soda-lime glass plates. The average peak molecular weight (Mp; after S-UV) of the sol portion of the adhesive in the separated adhesive layer was measured in the same manner as above. The results are shown in Table 2.

[0191] [Test Example 3] (Measurement of dynamic viscoelasticity) A 250 μm thick adhesive layer was produced by laminating multiple adhesive layers of the adhesive sheets produced in the Examples and Comparative Examples. The adhesive layer (250 μm) was irradiated with active energy rays (ultraviolet rays; UV) under the same active energy ray irradiation conditions as in Test Example 1, and the adhesive layer was cured. A cylindrical body with a diameter of 8 mm (height 0.25 mm) was punched out from the adhesive layer (250 μm) after active energy ray curing, and this was used as a sample.

[0192] The dynamic viscoelasticity of the above sample was measured in accordance with JIS K7244-1 using a viscoelasticity measuring device (manufactured by Anton Paar, product name "MCR302") by the torsional shear method under the following conditions, and the storage modulus G'(-15) (MPa; before S-UV) at -15°C, the storage modulus G'(23) (MPa; before S-UV) at 23°C, and the storage modulus G'(100) (MPa; before S-UV) at 100°C were observed. In addition, the peak temperature (°C) of the loss tangent tanδ (before S-UV: Tb) was also observed. The results are shown in Table 2. Measurement frequency: 1 Hz Measurement temperature range: -20°C to 140°C Heating rate: 4°C / min

[0193] Additionally, a 250 μm thick adhesive layer was produced by laminating multiple adhesive layers from the adhesive sheets produced in the Examples and Comparative Examples. A laminate was produced using this adhesive layer (thickness: 250 μm) in the same manner as in Test Example 1. The laminate was irradiated with active energy rays (ultraviolet rays; UV) under the same active energy ray irradiation conditions as in Test Example 1 to cure the adhesive layer. The resulting laminate was irradiated with ultraviolet rays (S-UV irradiation) under the same ultraviolet irradiation conditions as in Test Example 1. The adhesive layer of the laminate after S-UV irradiation was then separated from the two soda-lime glass plates. The dynamic viscoelasticity of the separated adhesive layer was measured in the same manner as above, and the storage modulus G'(-15) (MPa; after S-UV) at -15°C, the storage modulus G'(23) (MPa; after S-UV) at 23°C, and the storage modulus G'(100) (MPa; after S-UV) at 100°C were observed. The peak temperature (°C) of the loss tangent tan δ (after S-UV: Ta) was also observed. The results are shown in Table 2.

[0194] Furthermore, the value (Ta - Tb) was calculated by subtracting Tb from Ta obtained above. The results are shown in Table 2.

[0195] [Test Example 4] (Measurement of adhesive strength) The release sheet R2 was peeled off from the adhesive sheet produced in the Examples and Comparative Examples, and the exposed adhesive layer was attached to one of the easy-adhesion layers of a polyethylene terephthalate (PET) film (manufactured by Toyobo Co., Ltd., product name "Cosmoshine A4360", thickness: 100 μm) having easy-adhesion layers on both sides, to obtain a release sheet R1 / adhesive layer / PET film laminate. This laminate was cut into a width of 25 mm and a length of 100 mm, and this was used as a sample.

[0196] The release sheet R1 was peeled off from the sample in an environment of 23°C and 50% RH, and the exposed adhesive layer was attached to soda lime glass (manufactured by Nippon Sheet Glass Co., Ltd.), and then pressurized for 20 minutes at 0.5 MPa and 50°C in an autoclave manufactured by Kurihara Manufacturing Co., Ltd. Then, active energy rays (ultraviolet rays; UV) were irradiated through the soda lime glass under the same active energy ray irradiation conditions as in Test Example 1, to cure the adhesive layer.

[0197] After that, the adhesive strength (N / 25 mm) was measured using a tensile tester (Tensilon, manufactured by Orientec Co., Ltd.) at a peel speed of 300 mm / min and a peel angle of 180 degrees. The measurement was conducted under conditions other than those described here in accordance with JIS Z0237:2009. The results are shown in Table 2.

[0198] [Test Example 5] (Measurement of total light transmittance) A 250 μm thick adhesive layer was produced by laminating multiple adhesive layers of the adhesive sheets produced in the Examples and Comparative Examples. Using this adhesive layer (thickness: 250 μm), a laminate was produced in the same manner as in Test Example 1. The laminate was irradiated with active energy rays (ultraviolet rays; UV) under the same active energy ray irradiation conditions as in Test Example 1 to cure the adhesive layer, and this was used as a measurement sample.

[0199] For the above measurement sample, background measurement was performed using soda lime glass, and then the total light transmittance (%; before S-UV) was measured using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "NDH-5000") in accordance with JIS K7361-1:1997. The results are shown in Table 2. The total light transmittance of the adhesive layer before curing with active energy rays was also measured, and the same measurement result was obtained.

[0200] Test Example 6 (Haze Value Measurement) A measurement sample was prepared in the same manner as in Test Example 5. After background measurement was performed on the measurement sample using glass, the haze value (%; before S-UV) was measured using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "NDH-5000") in accordance with JIS K7136:2000. The results are shown in Table 2. The haze value of the adhesive layer before curing with active energy rays was also measured, and the same measurement result was obtained.

[0201] [Test Example 7] (Measurement of L*a*b*) A 250 μm thick adhesive layer was prepared by laminating multiple adhesive layers of the adhesive sheets produced in the Examples and Comparative Examples. A laminate was prepared using this adhesive layer (thickness: 250 μm) in the same manner as in Test Example 1. The laminate was irradiated with active energy rays (ultraviolet rays; UV) under the same active energy ray irradiation conditions as in Test Example 1 to cure the adhesive layer. The chromaticity b* (chromaticity b*1) of the resulting laminate, as defined by the CIE 1976 L*a*b* color system, was measured using a simultaneous photometric spectrophotometer (manufactured by Nippon Denshoku Industries Co., Ltd., product name "SQ2000"). The results are shown in Table 2.

[0202] The obtained laminate was also irradiated with ultraviolet light (S-UV irradiation) under the same ultraviolet irradiation conditions as in Test Example 1. The chromaticity b* (chromaticity b*2) of the adhesive layer after S-UV irradiation was measured in the same manner as above. The results are shown in Table 2.

[0203] Furthermore, the absolute value of the ratio (b*2 / b*1) of the chromaticity b*2 to the chromaticity b*1 obtained above was calculated. Based on these results, yellowing was evaluated according to the following criteria. The results are shown in Table 2. ◎: The absolute value of b*2 / b*1 was 3 or less. ○: The absolute value of b*2 / b*1 was more than 3 and 6 or less. △: The absolute value of b*2 / b*1 was more than 6 and 10 or less. ×: The absolute value of b*2 / b*1 was more than 10.

[0204] [Test Example 8] (Evaluation of Weather Resistance) A 250 μm thick adhesive layer was produced by laminating multiple adhesive layers of the adhesive sheets produced in the Examples and Comparative Examples. A laminate was produced in the same manner as in Test Example 1 using this adhesive layer (thickness: 250 μm). The laminate was irradiated with active energy rays (ultraviolet rays; UV) under the same conditions as in Test Example 1 to cure the adhesive layer. Next, the obtained laminate was irradiated with UV rays for 20 hours (light intensity: 7.2 kJ / cm 2 ), 40 hours (light intensity: 14.4 kJ / cm 2 ), 80 hours (light intensity: 28.8 kJ / cm 2 ), and 120 hours (light intensity: 43.2 kJ / cm 2The adhesive layer was then visually inspected and its weather resistance was evaluated based on the following criteria. The results are shown in Table 2. ⊚: No needle-like cracks occurred, and no bubbles, lifting, or peeling occurred. ◯: No needle-like cracks occurred, but some bubbles occurred. ×: Needle-like cracks occurred.

[0205] Test Example 9 (Evaluation of Blister Resistance) The release sheet R2 was peeled off from the adhesive sheets produced in the Examples and Comparative Examples, and the exposed adhesive layer was bonded to the PC plate side of a plastic plate (manufactured by Mitsubishi Gas Chemical Company, Inc., product name "Iupilon Sheet MR58U", thickness: 0.7 mm) consisting of a polycarbonate (PC) plate and a polymethyl methacrylate (PMMA) layer laminated thereon. The release sheet R1 was then peeled off from the adhesive layer to expose the adhesive layer, and a transparent conductive film (manufactured by Oike Kogyo Co., Ltd., laminate of a PET film and an ITO layer (ITO-PET film), total thickness 125 μm) was bonded to the adhesive layer so that the ITO layer side was in contact with the adhesive layer. The sheet was then autoclaved for 20 minutes at 50°C and 0.5 MPa.

[0206] The adhesive layer of the obtained laminate was cured by irradiating it with active energy rays (ultraviolet rays; UV) through the transparent conductive film under the same conditions as in Test Example 1. Thereafter, the laminate was left to stand at normal pressure, 23°C, and 50% RH for 24 hours, and this was used as a sample.

[0207] The obtained sample was stored for 72 hours under high temperature and high humidity conditions of 85°C and 85% RH. Thereafter, the condition of the interface between the adhesive layer and the adherend (plastic plate) was visually inspected, and blister resistance was evaluated according to the following criteria. The results are shown in Table 2. ○: No bubbles, lifting, or peeling occurred. △: Bubbles less than 1 mm in diameter occurred, but no lifting or peeling occurred. ×: Bubbles, lifting, or peeling occurred throughout the sample.

[0208]

[0209]

[0210] As can be seen from Table 2, the adhesive sheets produced in the Examples were able to suppress the occurrence of needle-like cracks even when irradiated with high-intensity UV light for long periods of time (20 hours, 40 hours, and 80 hours), and had excellent weather resistance. In particular, the adhesive sheets of Examples 2 to 5, which used a UV absorber, light stabilizer, or antioxidant, were able to suppress the occurrence of needle-like cracks even when irradiated with high-intensity UV light for an even longer period of time (120 hours), and had even more excellent weather resistance.

[0211] The adhesive sheet of the present invention can be suitably used, for example, in the production of a display, for bonding a display component such as a protective panel to a desired display component.

[0212] REFERENCE SIGNS LIST 1 adhesive sheet 11 adhesive layer 12a, 12b release sheets 2 display body 21 first display body constituent member 22 second display body constituent member 3 print layer

Claims

1. Adhesives used for optical applications that contain oxygen absorbers.

2. The adhesive according to claim 1, wherein the oxygen absorber is a compound represented by the following general formula (I): (In the general formula (I), X and Y each independently represent a chalcogen atom; R 1 , R 2 , R 7 , and R 8 each independently represents an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an aryl group, or an aralkyl group; R 3 , R 4 , R 5 , and R 6 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an aryl group, or an aralkyl group. J represents a linking group made of an aliphatic hydrocarbon having 3 to 15 carbon atoms, and any carbon atom of the linking group may be substituted with an oxygen atom, and the linking group may have at least one substituent selected from the group consisting of a hydroxyl group, a (meth)acryloyloxy group, a styryloxy group, and an alkenyloxy group having 2 to 5 carbon atoms. n is an integer of 1 to 5. However, Y, R 5 , R 6 , R 7 , and R 8 When a plurality of are present, they may be different atoms or groups.

3. The adhesive according to claim 1, wherein the oxygen absorber is a compound represented by the following general formula (II): (In general formula (II), R 9 represents a hydrogen atom or a methyl group, R 10 R represents any one of a hydroxyl group, a (meth)acryloyloxy group, a styryloxy group, and an alkenyloxy group having 2 to 5 carbon atoms. 11 , R 12 , R 13 , and R 14 each independently represents an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an aryl group, or an aralkyl group.

4. The adhesive according to claim 1, wherein the oxygen absorber is a compound represented by the following formula (III):

5. The adhesive according to claim 1, which is an acrylic adhesive.

6. The adhesive according to claim 1, wherein the adhesive base is a (meth)acrylic ester polymer or a crosslinked product thereof.

7. The adhesive according to claim 1, which is an active energy ray-curable adhesive.

8. An adhesive sheet having an adhesive layer for bonding two members together, at least one of the members being an optical member, and the adhesive layer being made of an adhesive as defined in any one of claims 1 to 7.

9. The chromaticity b* of the adhesive layer after lamination, as defined by the CIE 1976 L*a*b* color system, is b*1, and the illuminance of the adhesive layer after lamination is 100 mW / cm 2 9. The adhesive sheet according to claim 8, characterized in that, when chromaticity b* defined by the CIE 1976 L*a*b* color system of the adhesive layer after irradiation with ultraviolet light of 100 nm for 120 hours is b*2, the absolute value of the ratio of b*2 to b*1 is 10 or less.

10. The adhesive sheet according to claim 8, characterized in that the adhesive sheet comprises two release sheets, and the adhesive layer is sandwiched between the release sheets so as to contact the release surfaces of the two release sheets.

11. An optical construction comprising at least two members bonded together with an adhesive layer, wherein at least one of the members is an optical member, and the adhesive layer is formed from the adhesive according to any one of claims 1 to 7.

12. A display comprising: one display component; another display component; and an adhesive layer for bonding said one display component and said other display component to each other, wherein said adhesive layer is formed from an adhesive layer of an adhesive sheet as described in claim 8.

13. The display according to claim 12, wherein both the one display member and the other display member are hard plates.

Citation Information

Patent Citations

  • Ultraviolet-curable hot-melt adhesive

    JP2019218480A

  • Nanoparticle-filled barrier adhesive composition

    JP2019524911A

  • Coating Materials with Oxygen Scavenger and / or Oxygen Indicator Function for Coating or Bonding and Products Produced Therewith

    US20090117389A1

  • Adhesive and luminescent element

    WO2006080500A1

  • Compound containing unsaturated double bond, oxygen absorber comprising same, and resin composition

    WO2019107252A1

Cited By

  • Adhesive, adhesive sheet, optical structure, and display body

    WO2025142277A1

  • Adhesive, adhesive sheet, optical structure, and display body

    WO2025203862A1