Solid electrolyte, preparation method thereof, and all-solid rechargeable battery comprising same
The application of a thin polysiloxane-based hydrophobic polymer coating on inorganic solid electrolytes addresses chemical instability and conductivity issues, enhancing the stability and performance of all-solid-state secondary batteries.
Patent Information
- Application Number
- PCT/KR2024/000409
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-01-09
- Publication Date
- 2024-10-03
AI Technical Summary
Inorganic solid electrolytes used in all-solid-state secondary batteries suffer from chemical instability due to moisture exposure, leading to deterioration and reduced ionic conductivity, which is costly to mitigate and limits their application.
A solid electrolyte with a thin coating layer of thermal decomposition products from a linear polysiloxane-based hydrophobic polymer is applied, enhancing atmospheric stability and minimizing conductivity loss.
The coated solid electrolyte exhibits improved lifespan characteristics and reduced ionic conductivity degradation, enabling more stable and efficient battery performance.
Smart Images

Figure KR2024000409_03102024_PF_FP_ABST
Abstract
Description
Solid electrolyte, method for manufacturing the same, and all-solid-state secondary battery comprising the same
[0001] The present invention relates to a solid electrolyte, a method for manufacturing the same, and an all-solid-state secondary battery including the same.
[0002] Lithium secondary batteries, which offer high energy density and portability, are primarily used as power sources for mobile information terminals such as mobile phones, laptops, and smartphones. Recently, active research is underway to utilize high-energy-density lithium secondary batteries as power sources for hybrid and electric vehicles, or as power storage devices.
[0003] Commercially available lithium secondary batteries use electrolytes containing flammable organic solvents, posing safety concerns that can lead to explosion or fire in the event of collisions, penetration, or other problems. Therefore, all-solid-state secondary batteries, which utilize solid electrolytes instead of the electrolyte, have been proposed. All-solid-state secondary batteries are composed entirely of solid materials, eliminating the risk of electrolyte leakage and explosion, making them safer. Furthermore, they facilitate the production of thin batteries, allowing for a reduced anode thickness, improving high-speed charge / discharge performance and enabling high-voltage operation and high-energy density.
[0004] Inorganic solid electrolytes, such as sulfide, oxide, and halide, are widely used. Inorganic solid electrolytes possess high ionic conductivity and, due to their soft mechanical properties, facilitate the formation of interparticle contact surfaces, making them a key solid electrolyte material. However, inorganic solid electrolytes are known to deteriorate due to their poor chemical stability, reacting with atmospheric moisture to form compounds such as hydrogen sulfide and hydrogen chloride.
[0005] In order to suppress the deterioration of the inorganic solid electrolyte, it is necessary to handle the material in a specific space such as a glove box with an inert gas atmosphere or a dry room from which moisture has been removed. However, this not only causes an increase in process costs, but also has limitations in preventing continuous deterioration because the inorganic solid electrolyte reacts with a small amount of moisture even in the above space.
[0006] To address this, research has been conducted to improve chemical stability and suppress deterioration due to reaction with atmospheric moisture by adding metal oxide materials to inorganic solid electrolytes or replacing some of the elements with other elements. However, although adding metal oxide materials to inorganic solid electrolytes is effective in suppressing the generation of hydrogen sulfide and other gases, it not only reduces the ionic conductivity of the solid electrolyte, but also has limitations in suppressing deterioration of the solid electrolyte material itself. Furthermore, although suppressing deterioration by replacing some of the elements in an inorganic solid electrolyte with other elements is effective in suppressing deterioration of the solid electrolyte material itself, there are limitations such as a decrease in the ionic conductivity of the solid electrolyte, the use of toxic elements such as arsenic, and limitations in applicable structures.
[0007] Therefore, there is an urgent need to develop a technology that 1) can be applied to various inorganic solid electrolytes such as sulfide, oxide, and halide, 2) significantly reduces the decrease in ionic conductivity of the solid electrolyte, 3) is effective in suppressing deterioration of the solid electrolyte material itself, 4) does not use toxic elements, and 5) can be applied to materials of various structures.
[0008] A solid electrolyte is provided that improves the atmospheric stability of an inorganic solid electrolyte, suppresses deterioration of the material itself, and reduces the decrease in ionic conductivity.
[0009] In one embodiment, a solid electrolyte is provided, which comprises solid electrolyte particles and a coating layer positioned on the surface of the solid electrolyte particles, wherein the coating layer comprises a thermal decomposition product of a linear polysiloxane-based hydrophobic polymer, and the coating layer has a thickness of 1 nm to 50 nm.
[0010] In another embodiment, a method for manufacturing a solid electrolyte is provided, which includes introducing solid electrolyte particles and a linear polysiloxane-based hydrophobic polymer into a vacuum tube without contacting each other, and heat-treating the vacuum tube to vapor-deposit the linear polysiloxane-based hydrophobic polymer on the surface of the solid electrolyte particles.
[0011] In another embodiment, an all-solid-state secondary battery including the solid electrolyte is provided.
[0012] A solid electrolyte according to an embodiment of the present invention has excellent atmospheric stability and a small decrease in ionic conductivity, so an all-solid-state secondary battery using the solid electrolyte can exhibit excellent electrochemical characteristics such as lifespan characteristics.
[0013] Figures 1 and 2 are cross-sectional views schematically showing an all-solid-state secondary battery according to one embodiment.
[0014] Figure 3 is an ultra-low temperature transmission electron microscope image of the surface of the solid electrolyte manufactured in Example 1.
[0015] Figure 4 shows the results of X-ray photoelectron spectroscopy analysis of the solid electrolytes of Comparative Example 1 and Example 1.
[0016] Figure 5 shows the results of thermogravimetric analysis for the solid electrolytes of Comparative Example 1 and Example 1.
[0017] Below, specific implementation examples are described in detail to facilitate their implementation by those skilled in the art. However, the present invention may be implemented in various different forms and is not limited to the implementation examples described herein.
[0018] The terminology used herein is for the purpose of describing exemplary embodiments only and is not intended to limit the present invention. Singular expressions include plural expressions unless the context clearly dictates otherwise.
[0019] Here, “combination of these” means a mixture, laminate, composite, copolymer, alloy, blend, reaction product, etc. of the components.
[0020] It should be understood that the terms "include," "comprising," or "having" herein are intended to specify the presence of a feature, number, step, component, or combination thereof, but do not preclude the possibility of the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.
[0021] To clearly illustrate various layers and regions in the drawings, their thicknesses are enlarged, and similar parts are designated by the same drawing reference numerals throughout the specification. When an element such as a layer, film, region, or plate is said to be "over" or "on" another element, this includes not only the case where it is "directly over" the other element, but also the case where there are other elements in between. Conversely, when an element is said to be "directly over" another element, it means that there are no other elements in between.
[0022] Also, here, “layer” includes not only the shape formed on the entire surface when observed in a plan view, but also the shape formed on a portion of the surface.
[0023] The average particle size can be measured by methods well known to those skilled in the art, for example, by measuring with a particle size analyzer, or by measuring with a transmission electron microscope image or a scanning electron microscope image. Alternatively, the average particle size can be obtained by measuring using dynamic light scattering, performing data analysis, counting the number of particles for each particle size range, and calculating from the counted number. Unless otherwise defined, the average particle size can mean the diameter (D50) of particles in a particle size distribution that have a cumulative volume of 50% by volume. In addition, unless otherwise defined, the average particle size can be obtained by randomly measuring the sizes (diameters or major axis lengths) of about 20 particles in a scanning electron microscope image to obtain a particle size distribution, and taking the diameter (D50) of particles in the particle size distribution that have a cumulative volume of 50% by volume as the average particle size.
[0024] Here, “or” is not interpreted in an exclusive sense, for example, “A or B” is interpreted to include A, B, A+B, etc.
[0025] “Metal” is interpreted as a concept that includes common metals, transition metals, and metalloids (semi-metals).
[0026] solid electrolyte
[0027] In one embodiment, a solid electrolyte is provided, which comprises solid electrolyte particles and a coating layer positioned on the surface of the solid electrolyte particles, wherein the coating layer comprises a thermal decomposition product of a linear polysiloxane-based hydrophobic polymer, and the coating layer has a thickness of 1 nm to 50 nm. Here, the solid electrolyte particles correspond to a type of core, and the final solid electrolyte can be referred to as a coated solid electrolyte.
[0028] coating layer
[0029] In the above solid electrolyte, the coating layer is formed by a type of vapor deposition method described below, and is different in composition and shape from those coated by general methods such as wet coating or dry coating. The coating layer may be formed by, for example, vacuum deposition. In the solid electrolyte manufactured according to one embodiment, the coating layer is very thin, such as 1 nm to 50 nm in thickness, and the thickness is very uniform, so that the thickness deviation is small. Accordingly, contact between the solid electrolyte particles and moisture in the air can be effectively suppressed, thereby fundamentally suppressing deterioration of the solid electrolyte, and significantly reducing the degree to which the ionic conductivity of the solid electrolyte decreases due to the coating.
[0030] The coating layer may be in the form of a film that completely surrounds the surface of the solid electrolyte particles. In addition, the thickness of the coating layer may be 1 nm to 50 nm, for example, 1 nm to 40 nm, 2 nm to 30 nm, 3 nm to 20 nm, 4 nm to 15 nm, or 5 nm to 10 nm. When the coating layer is formed with such a thin thickness, the reduction in ionic conductivity of the solid electrolyte due to the coating can be minimized, and the solid electrolyte particles can be fundamentally prevented from coming into contact with moisture in the air. Here, the thickness of the coating layer may be measured from an electron microscope image of a cross-section of the solid electrolyte, and for example, may be measured by photographing a cross-section of the solid electrolyte cut with a focused ion beam (FIB) using a cryogenic transmission electron microscope (Cyro-TEM). In addition, the thickness of the coating layer may be obtained by randomly measuring the thickness of 10 places in an electron microscope image of a cross-section of the solid electrolyte and calculating the arithmetic average thereof.
[0031] The coating layer is characterized by having a uniform thickness. For example, the deviation of the thickness of the coating layer in one solid electrolyte particle may be 30% or less, for example, 25% or less or 20% or less. Here, the deviation of the thickness of the coating layer may mean that, in an electron microscope image of a cross-section of the solid electrolyte, the thickness of about 10 points on the surface of one solid electrolyte particle is measured, an arithmetic mean is calculated, and then the absolute value of the difference between one data point and the arithmetic mean is divided by the arithmetic mean and multiplied by 100. As another example, the standard deviation of the thickness of the coating layer in one solid electrolyte particle may be 5 nm or less, for example, 4 nm or less, 3 nm or less, or 2 nm or less. The standard deviation of the thickness of the coating layer may likewise be calculated by measuring the thickness of about 10 points in an electron microscope image and calculating the standard deviation. The deviation or standard deviation of the coating layer thickness satisfying the above range means that a coating layer of uniform thickness is well formed in a film form on the surface of the solid electrolyte particles, and accordingly, the exposure of the solid electrolyte particles to the air is fundamentally blocked, thereby minimizing the decrease in lithium ion conductivity due to the coating.
[0032] The content of the coating layer may be comprised in an amount of 1 wt% to 5 wt% based on 100 wt% of the solid electrolyte, for example, 2 wt% to 5 wt% or 3 wt% to 5 wt%. When the weight of the coating layer satisfies the above range, it is suitable for reducing the decrease in ionic conductivity while blocking the exposure of the solid electrolyte to air.
[0033] The coating layer is characterized in that the linear polysiloxane-based hydrophobic polymer includes a thermal decomposition product. In the vapor deposition process described below, the linear polysiloxane-based hydrophobic polymer is thermally decomposed, and the thermal decomposition product of the polymer exists in the final coating layer. In the thermal decomposition product of the polymer, Si-O bonds and the like can be detected. For example, in X-ray photoelectron spectroscopy (XPS) analysis of the solid electrolyte according to one embodiment, Si-O peaks and the like can be detected. For example, in the XPS analysis graph, a peak may appear at 102 ± 0.1 eV, which is the position of Si-O 2p3 / 2, and a peak may appear at 102.6 ± 0.1 eV, which is the position of Si-O 2p1 / 2.
[0034] The above linear polysiloxane hydrophobic polymer refers to a polymer having a main chain centered on silicon and oxygen bonds. In addition, the linear polysiloxane hydrophobic polymer is distinguished from polymers having cyclic, branched, cross-linked, or network-like structures, and is a polymer connected in the form of a single long chain. Such linear polysiloxane hydrophobic polymers are most suitable for thinly and uniformly coating the surface of solid electrolyte particles using a vapor deposition method.
[0035] In addition, the polymer is hydrophobic, which means that it does not easily combine with water molecules, and may mean that the contact angle between any surface and a water droplet is greater than 90°. According to one embodiment, the solid electrolyte is coated with a thermal decomposition product of the hydrophobic polymer, thereby effectively blocking the solid electrolyte particles from contacting moisture in the air.
[0036] The linear polysiloxane-based hydrophobic polymer may be, for example, poly(dimethylsiloxane), poly(methylhydrosiloxane), poly(dimethylsiloxane-co-alkylmethylsiloxane), poly(dimethylsiloxane having a terminal vinyl group, poly(dimethylsiloxane having a terminal bis(hydroxylalkyl) group, poly(dimethylsiloxane having a terminal bis(3-aminopropyl) group, poly(dimethylsiloxane having a terminal hydroxyl group), or a combination thereof. Here, the alkyl may be, for example, C1 to C10 alkyl, or C1 to C5 alkyl, or C2 to C5 alkyl. The designation C10, etc. above indicates the number of carbon atoms, and C10 alkyl means alkyl having 10 carbon atoms.
[0037] Meanwhile, the linear polysiloxane-based hydrophobic polymer may contain a fluorine group. For example, the linear polysiloxane-based hydrophobic polymer may additionally contain a CF bond, in which case the hydrophobicity of the polymer is further enhanced, thereby more effectively blocking the solid electrolyte from contacting moisture in the air. The fluorine-containing polymer can be manufactured by adding a substance having a CF bond to the linear polysiloxane-based hydrophobic polymer matrix through techniques such as crosslinking and grafting.
[0038] Specific examples of linear polysiloxane-based superhydrophobic polymers containing fluorine groups include, but are not limited to, 1H,1H,2H,2H-perfluorodecyltriethoxysilane, 1H,1H,2H,2H-perfluorododecyltrichlorosilane, 1H,1H,2H-perfluorooctyltridecoxysilane, or combinations thereof.
[0039] The number average molecular weight of the linear polysiloxane-based hydrophobic polymer may be 3,000 g / mol to 50,000 g / mol, for example, 5,000 g / mol to 50,000 g / mol, or 5,000 g / mol to 40,000 g / mol, or 10,000 g / mol to 30,000 g / mol. When the molecular weight of the polymer satisfies the above range, it is suitable for vapor deposition on the surface of solid electrolyte particles, can minimize a decrease in ionic conductivity of the solid electrolyte, and can improve the atmospheric stability of the solid electrolyte by reducing the degree of decrease in ionic conductivity of the solid electrolyte due to exposure to the atmosphere.
[0040] The above coating layer may be non-crystalline. By uniformly coating an amorphous coating layer containing a thermal decomposition product of a linear polysiloxane-based hydrophobic polymer with a very thin thickness, the solid electrolyte particles can be effectively blocked from the atmosphere, while at the same time minimizing the decrease in ionic conductivity.
[0041] solid electrolyte particles
[0042] The above solid electrolyte particles may include an inorganic solid electrolyte, for example, a sulfide-based solid electrolyte, an oxide-based solid electrolyte, a halide-based solid electrolyte, or a combination thereof. The above-described coating layer can be effectively deposited on the surface of various types of inorganic solid electrolyte particles.
[0043] Sulfide-based solid electrolyte
[0044] The above solid electrolyte particles may be, for example, sulfide-based solid electrolyte particles having excellent ion conductivity. The sulfide-based solid electrolyte particles may be, for example, Li2S-P2S5, Li2S-P2S5--LiX (X is a halogen element, for example, I or Cl), Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n (m, n are integers, Z is Ge, Zn or Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q (p, q are integers, and M is P, Si, Ge, B, Al, Ga or In), or a combination thereof.
[0045] Such sulfide-based solid electrolytes can be obtained, for example, by mixing Li2S and P2S5 in a molar ratio of 50:50 to 90:10, or 50:50 to 80:20, and optionally heat-treating them. Within the above mixing ratio range, a sulfide-based solid electrolyte having excellent ionic conductivity can be produced. Here, the ionic conductivity can be further improved by further including other components such as SiS2, GeS2, and B2S3.
[0046] Methods for mixing sulfur-containing raw materials for producing sulfide-based solid electrolytes include mechanical milling or the solution method. Mechanical milling involves placing raw materials in a ball mill reactor and vigorously stirring them to finely atomize and mix them. Using the solution method, the raw materials are mixed in a solvent to obtain a solid electrolyte as a precipitate. Furthermore, heat treatment after mixing can solidify the crystals of the solid electrolyte and improve ionic conductivity. For example, a sulfide-based solid electrolyte can be produced by mixing sulfur-containing raw materials and heat-treating them twice or more, resulting in a sulfide-based solid electrolyte with high ionic conductivity and robustness.
[0047] According to one embodiment, a sulfide-based solid electrolyte can be manufactured through, for example, a first heat treatment in which sulfur-containing raw materials are mixed and calcined at 120°C to 350°C, and a second heat treatment in which the first heat treatment result is mixed and calcined at 350°C to 800°C. The first heat treatment and the second heat treatment can each be performed in an inert gas or nitrogen atmosphere. The first heat treatment can be performed for 1 to 10 hours, and the second heat treatment can be performed for 5 to 20 hours. The first heat treatment can have the effect of milling small raw materials, and the second heat treatment can synthesize the final solid electrolyte. Through two or more such heat treatments, a high-performance sulfide-based solid electrolyte with high ionic conductivity and robustness can be obtained, and such a solid electrolyte can be said to be suitable for mass production. The temperature of the first heat treatment may be, for example, 150°C to 330°C, or 200°C to 300°C, and the temperature of the second heat treatment may be, for example, 380°C to 700°C, or 400°C to 600°C.
[0048] For example, the sulfide-based solid electrolyte may include an argyrodite-type sulfide. The argyrodite-type sulfide may be, for example, Li aM b P c S d A e (wherein a, b, c, d, and e are all 0 or more and 12 or less, M is Ge, Sn, Si, or a combination thereof, and A is F, Cl, Br, or I) and can be expressed by the chemical formula, and a specific example is Li 7-x PS 6-x A x (x is 0.2 or more and 1.8 or less, and A is F, Cl, Br, or I) can be expressed by the chemical formula. The above argyrodite-type sulfide is specifically Li3PS4, Li7P3S 11 , Li7PS6, Li6PS5Cl, Li6PS5Br, Li 5.8 PS 4.8 Cl 1.2 , Li 6.2 PS 5.2 Br 0.8 It could be the back.
[0049] Sulfide-based solid electrolytes containing these argyrodite-type sulfides have an ionic conductivity of 10 that of typical liquid electrolytes at room temperature. -4 10 inland -2 It has a high ionic conductivity approaching the S / cm range, can form a close bond between a positive electrode active material and a solid electrolyte without causing a decrease in ionic conductivity, and further can form a close interface between an electrode layer and a solid electrolyte layer. An all-solid-state secondary battery including this can have improved battery performance, such as rate characteristics, Coulombic efficiency, and cycle life characteristics.
[0050] An argyrodite-type sulfide-based solid electrolyte can be manufactured, for example, by mixing lithium sulfide and phosphorus sulfide, optionally a lithium halide. After mixing these, a heat treatment may be performed. The heat treatment may include, for example, two or more heat treatment steps. Here, manufacturing an argyrodite-type sulfide-based solid electrolyte may include, for example, a first heat treatment of mixing raw materials and calcining at 120°C to 350°C, and a second heat treatment of mixing the resultant of the first heat treatment again and calcining at 350°C to 800°C.
[0051] Oxide-based solid electrolyte
[0052] The above solid electrolyte particles may be oxide-based inorganic solid electrolyte particles, and the oxide-based solid electrolyte may be, for example, Li 1+x Ti 2-x Al(PO4)3(LTAP)(0≤x≤4), Li 1+x+y Al x Ti 2-x Si y P 3-y O 12 (0 <x<2, 0≤y<3), BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT)(0≤x<1, 0≤y<1), PB(Mg3Nb 2 / 3 )O3-PbTiO3(PMN-PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, lithium phosphate (Li3PO4), lithium titanium phosphate (Li x Ti y (PO4)3, 0 <x<2, 0<y<3), Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0≤x≤1, 0≤y≤1), lithium lanthanum titanate (Lix La y TiO3, 0 <x<2, 0<y<3), Li2O, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2계 세라믹스, 가넷(Garnet)계 세라믹스 Li 3+x La3M2O 12 (M= Ta, Te, Nb, or Zr; x is an integer from 1 to 10), or mixtures thereof.
[0053] Halide-based solid electrolyte
[0054] The above solid electrolyte particles may be a halide solid electrolyte. A halide-based solid electrolyte contains a halogen element as a main component, and may mean that the ratio of the halide element to all elements constituting the solid electrolyte is 50 mol% or more, 70 mol% or more, 90 mol% or more, or 100 mol%. For example, the halide-based solid electrolyte may not contain a sulfur element.
[0055] The above halide-based solid electrolyte may contain a lithium element, a metal element other than lithium, and a halogen element. The metal element other than lithium may be Al, As, B, Bi, Ca, Cd, Co, Cr, Fe, Ga, Hf, In, Mg, Mn, Ni, Sb, Sc, Sn, Ta, Ti, Y, Zn, Zr, or a combination thereof. The halogen element may be F, Cl, Br, I, or a combination thereof, and may be Cl, Br, or a combination thereof, for example. The halide-based solid electrolyte may contain, for example, Li a M 1 c M 2 d X b (M 1 and M 2are each independently Al, As, B, Bi, Ca, Cd, Co, Cr, Fe, Ga, Hf, In, Mg, Mn, Ni, Sb, Sc, Sn, Ta, Ti, Y, Zn, Zr, or a combination thereof, X is F, Cl, Br, I, or a combination thereof, a, b are each independently in the range of 0.1 to 10, and c, d may be in the range of 0 to 1.) The halide-based solid electrolyte may be represented by, for example, Li2ZrCl6, Li 2.7 Y 0.7 Zr 0.3 Cl6, Li 2.5 Y 0.5 Zr 0.5 Cl6, Li 2.5 In 0.5 Zr 0.5 Cl6, Li2In 0.5 Zr 0.5 Cl6, Li3YBr6, Li3YCl6, Li3YBr2Cl4, Li3YbCl6, Li 2.6 Hf 0.4 Yb 0.6 Cl6, or combinations thereof, but is not limited thereto.
[0056] The average particle diameter (D50) of the solid electrolyte particles may be 5.0 ㎛ or less, for example, 0.1 ㎛ to 5.0 ㎛, 0.5 ㎛ to 5.0 ㎛, 0.5 ㎛ to 4.0 ㎛, 0.5 ㎛ to 3.0 ㎛, 0.5 ㎛ to 2.0 ㎛, or 0.5 ㎛ to 1.0 ㎛. The solid electrolyte particles may be small particles having a size of 0.1 ㎛ to 1.5 ㎛, large particles having a size of 2.0 ㎛ to 5.0 ㎛, or a mixture thereof. The average particle diameter of the solid electrolyte particles may be measured by an electron microscope image, and for example, a particle size distribution may be obtained by measuring the size (diameter or major axis length) of about 20 particles in a scanning electron microscope image, and D50 may be calculated therefrom.
[0057] Method for manufacturing solid electrolyte
[0058] In one embodiment, a method for manufacturing a solid electrolyte is provided, which includes introducing solid electrolyte particles and a linear polysiloxane-based hydrophobic polymer into a vacuum tube without contacting each other, and heat-treating the vacuum tube to vapor-deposit the linear polysiloxane-based hydrophobic polymer on the surface of the solid electrolyte particles.
[0059] Through the above method, the thermal decomposition product of the linear polysiloxane-based hydrophobic polymer can be coated on the surface of the solid electrolyte particles in a very uniform and thin thickness. Since the method for manufacturing a solid electrolyte according to one embodiment does not use a solvent, it can suppress the deterioration of the solid electrolyte that occurs during the coating process, and since a very thin and uniform coating layer can be formed, the reduction in lithium ion conductivity of the solid electrolyte can be minimized. In addition, according to the above manufacturing method, it is possible to obtain the solid electrolyte in a powder state after coating, which is economical and simple and is further advantageous in suppressing the deterioration of the solid electrolyte.
[0060] Since the solid electrolyte particles and the linear polysiloxane-based hydrophobic polymer themselves are as described above, a detailed description thereof will be omitted. When introducing them into a vacuum tube, the solid electrolyte particles and the linear polysiloxane-based hydrophobic polymer may be introduced at a weight ratio of 95:5 to 40:60, for example, at a weight ratio of 91:9 to 40:60, 90:10 to 40:60, 85:15 to 50:50, or 83:17 to 50:50. When introduced at such a weight ratio, a coating layer having an appropriate content can be formed at an appropriate thickness, and a decrease in ionic conductivity of the solid electrolyte can be minimized. In addition, the degree of decrease in ionic conductivity due to exposure to the atmosphere can be lowered, thereby improving atmospheric stability.
[0061] The above vapor deposition can be considered a type of vacuum deposition. During the coating process, exposure of the solid electrolyte particles to the atmosphere must be prevented, and heat treatment in a vacuum atmosphere is essential for the successful deposition of the linear polysiloxane-based hydrophobic polymer. The heat treatment in the vacuum tube can be performed in a vacuum atmosphere or at an atmospheric pressure of 0.1 mmHg or less.
[0062] In addition, heat treatment at a constant temperature is required for uniform vapor deposition of the linear polysiloxane-based hydrophobic polymer. The heat treatment may be performed in a temperature range of 150°C to 400°C, for example, 150°C to 350°C, or 200°C to 300°C. By performing heat treatment in the above temperature range, a thin and uniform coating layer can be formed. For example, if the heat treatment temperature is too low, the vapor deposition reaction rate of the polymer may be low, resulting in a long reaction time or incomplete deposition. On the other hand, if the heat treatment temperature is too high, the vapor deposition reaction rate of the polymer may be high, resulting in the formation of an uneven coating layer.
[0063] In addition, an appropriate level of heat treatment time is required for efficient vapor deposition of the linear polysiloxane-based hydrophobic polymer. The heat treatment may be performed for 0.5 to 6 hours, for example, 0.5 to 5 hours, 0.5 to 4 hours, or 0.5 to 3 hours. By performing the heat treatment for the above-mentioned time range, a thin and uniform coating layer can be effectively formed. For example, if the heat treatment time is too long, the process time becomes longer and costs increase, and if the heat treatment time is too short, an uneven coating layer may be formed.
[0064] All-solid-state secondary battery
[0065] In one embodiment, an all-solid-state secondary battery comprising the aforementioned solid electrolyte is provided. The all-solid-state secondary battery comprises a positive electrode, a negative electrode, and a solid electrolyte layer positioned between the positive electrode and the negative electrode. The solid electrolyte may be included in one or more of the positive electrode, the negative electrode, and the solid electrolyte layer.
[0066] FIG. 1 is a cross-sectional view of an all-solid-state secondary battery according to an embodiment. Referring to FIG. 1, the all-solid-state secondary battery (100') may have a structure in which an electrode assembly in which a negative electrode (400) including a negative electrode collector (401) and a negative electrode active material layer (403), a solid electrolyte layer (300), and a positive electrode (200) including a positive electrode active material layer (203) and a positive electrode collector (201) are laminated is housed in a battery case. The all-solid-state secondary battery (100') may further include an elastic layer (500) on the outer side of at least one of the positive electrode (200) and the negative electrode (400). Although FIG. 1 illustrates one electrode assembly including a negative electrode (400), a solid electrolyte layer (300), and a positive electrode (200), an all-solid-state secondary battery may be manufactured by laminating two or more electrode assemblies.
[0067] solid electrolyte layer
[0068] The solid electrolyte layer may include the aforementioned solid electrolyte and optionally further include a binder.
[0069] The binder may include, for example, nitrile-butadiene rubber, hydrogenated nitrile-butadiene rubber, styrene-butadiene rubber, acrylated styrene-butadiene rubber, acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluoroelastomer, polydimethylsiloxane, polyethylene oxide, polyvinylpyrrolidone, polyvinylpyridine, chlorosulfonated polyethylene, polyvinyl alcohol, polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyethylene, polypropylene, ethylene propylene copolymer, ethylene propylene diene copolymer, polyamideimide, polyimide, poly(meth)acrylate, polyacrylonitrile, polystyrene, polyurethane, or a combination thereof.
[0070] The above solid electrolyte layer may optionally further include an alkali metal salt, and / or an ionic liquid, and / or a conductive polymer.
[0071] The above alkali metal salt may be, for example, a lithium salt. The content of the lithium salt in the solid electrolyte layer may be 1 M or more, for example, 1 M to 4 M. In this case, the lithium salt may improve ion conductivity by enhancing the lithium ion mobility of the solid electrolyte layer.
[0072] The above lithium salts include, for example, LiSCN, LiN(CN)2, Li(CF3SO2)3C, LiC4F9SO3, LiN(SO2CF2CF3)2, LiCl, LiF, LiBr, LiI, LiB(C2O4)2, LiBF4, LiBF3(C2F5), lithium bis(oxalato)borate (LiBOB), lithium oxalyldifluoroborate (LIODFB), lithium difluoro(oxalato)borate (LiDFOB), lithium bis(trifluoro methanesulfonyl)imide (LiTFSI, LiN(SO2CF3)2), lithium bis(fluorosulfonyl)imide (LiFSI, It may include LiN(SO2F)2), LiCF3SO3, LiAsF6, LiSbF6, LiClO4 or mixtures thereof.
[0073] In addition, the lithium salt may be an imide-based one, and for example, the imide-based lithium salt may include lithium bis(trifluoro methanesulfonyl)imide (LiTFSI, LiN(SO2CF3)2), lithium bis(fluorosulfonyl)imide (LiFSI, LiN(SO2F)2). The lithium salt may maintain or improve ionic conductivity by appropriately maintaining chemical reactivity with an ionic liquid.
[0074] The above ionic liquid has a melting point below room temperature and is a salt or room-temperature molten salt that is liquid at room temperature and consists only of ions.
[0075] The above ionic liquid comprises a) one or more cations selected from ammonium, pyrrolidinium, pyridinium, pyrimidinium, imidazolium, piperidinium, pyrazolium, oxazolium, pyridazinium, phosphonium, sulfonium, triazolium, and mixtures thereof, and b) BF4. - , PF6 - , AsF6 - , SbF6 - , AlCl4 - , HSO4 - , ClO4 - , CH3SO3 - , CF3CO2 - , Cl - , Br - , I - , BF4 - , SO4 - , CF3SO3 - , (FSO2)2N - , (C2F5SO2)2N - , (C2F5SO2)(CF3SO2)N - , and (CF3SO2)2N - It may be a compound containing one or more anions selected from among.
[0076] The ionic liquid may be at least one selected from the group consisting of, for example, N-methyl-N-propylpyrrolidinium bis(trifluoromethanesulfonyl)imide, N-butyl-N-methylpyrrolidinium bis(3-trifluoromethylsulfonyl)imide, 1-butyl-3-methylimidazolium bis(trifluoromethylsulfonyl)amide, and 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)amide.
[0077] In the above solid electrolyte layer, the weight ratio of the solid electrolyte and the ionic liquid may be 0.1:99.9 to 90:10, for example, 10:90 to 90:10, 20:80 to 90:10, 30:70 to 90:10, 40:60 to 90:10, or 50:50 to 90:10. A solid electrolyte layer satisfying the above range can maintain or improve ionic conductivity by improving the electrochemical contact area with the electrode. Accordingly, the energy density, discharge capacity, rate characteristics, etc. of the all-solid-state secondary battery can be improved.
[0078] cathode
[0079] An anode for an all-solid-state secondary battery comprises a current collector and a negative electrode active material layer positioned on the current collector. The negative electrode active material layer comprises a negative electrode active material, may further comprise a binder and / or a conductive material, and may optionally comprise the solid electrolyte described above.
[0080] The above negative electrode active material includes a material capable of reversibly intercalating / deintercalating lithium ions, lithium metal, an alloy of lithium metal, a material capable of doping and dedoping lithium, or a transition metal oxide.
[0081] The material capable of reversibly intercalating / deintercalating the lithium ions may include a carbon-based negative electrode active material, for example, crystalline carbon, amorphous carbon, or a combination thereof. Examples of the crystalline carbon include graphite such as natural graphite or artificial graphite in an amorphous, plate-like, flake-like, spherical, or fibrous form, and examples of the amorphous carbon include soft carbon or hard carbon, mesophase pitch carbide, calcined coke, and the like.
[0082] As the above lithium metal alloy, an alloy of lithium and a metal selected from the group consisting of Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn can be used.
[0083] As the material capable of doping and dedoping the lithium, a Si-based negative electrode active material or a Sn-based negative electrode active material can be used, and the Si-based negative electrode active material may be silicon, a silicon-carbon composite, or SiO. x (0 < x < 2), Si-Q alloy (wherein Q is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof, and is not Si), Sn-based negative electrode active materials include Sn, SnO2, Sn-R alloy (wherein R is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof, and is not Sn), and at least one of these may be mixed with SiO2 for use. The above elements Q and R may be selected from the group consisting of Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.
[0084] For example, the negative active material may include silicon-carbon composite particles. The average particle diameter (D50) of the silicon-carbon composite particles may be, for example, 0.5 μm to 20 μm. The average particle diameter (D50) is measured by a particle size analyzer and refers to the diameter of particles having a cumulative volume of 50% by volume in a particle size distribution. With respect to 100 wt% of the silicon-carbon composite particles, silicon may be included in an amount of 10 wt% to 60 wt% and carbon may be included in an amount of 40 wt% to 90 wt%. The silicon-carbon composite particles may include, for example, a core including silicon particles and a carbon coating layer positioned on a surface of the core. The average particle diameter (D50) of the silicon particles in the core may be, for example, 10 nm to 1 μm, or 10 nm to 200 nm. The silicon particles may exist as silicon alone, in the form of a silicon alloy, or in an oxidized form. The oxidized form of silicon is SiO x (0 <x<2)로 표시될 수 있다. 또한, 상기 탄소 코팅층의 두께는 약 5 nm 내지 100 nm일 수 있다.
[0085] For example, the silicon-carbon composite particle may include a core including silicon particles and crystalline carbon, and a carbon coating layer located on the surface of the core and including amorphous carbon. For example, in the silicon-carbon composite particle, the amorphous carbon may not be present in the core but may be present only in the carbon coating layer. The crystalline carbon may be artificial graphite, natural graphite, or a combination thereof, and the amorphous carbon may be formed from coal pitch, mesophase pitch, petroleum pitch, coal oil, petroleum heavy oil, or a polymer resin (phenol resin, furan resin, polyimide resin, etc.). At this time, the content of the crystalline carbon may be 10 wt% to 70 wt%, and the content of the amorphous carbon may be 20 wt% to 40 wt% with respect to 100 wt% of the silicon-carbon composite particle.
[0086] In the above silicon-carbon composite particle, the core may include a void in the central portion. The radius of the void may be 30% to 50% of the radius of the silicon-carbon composite particle.
[0087] The silicon-carbon composite particles described above can effectively suppress problems such as volume expansion, structural collapse, or particle crushing due to charge and discharge, thereby preventing the phenomenon of conductive path disconnection, realizing high capacity and high efficiency, and are advantageous for use under high voltage or fast charging conditions.
[0088] The above Si-based negative electrode active material or Sn-based negative electrode active material can be used in combination with a carbon-based negative electrode active material. When the Si-based negative electrode active material or Sn-based negative electrode active material and the carbon-based negative electrode active material are used in combination, the mixing ratio can be 1:99 to 90:10 by weight.
[0089] The content of the negative active material in the above negative active material layer may be 95 wt% to 99 wt% with respect to the total weight of the negative active material layer.
[0090] In one embodiment, the negative electrode active material layer further includes a binder and may optionally further include a conductive material. The content of the binder in the negative electrode active material layer may be 1 wt% to 5 wt% based on the total weight of the negative electrode active material layer. In addition, when the negative electrode active material layer further includes a conductive material, the negative electrode active material layer may include 90 wt% to 98 wt% of the negative electrode active material, 1 wt% to 5 wt% of the binder, and 1 wt% to 5 wt% of the conductive material.
[0091] The above binder serves to adhere the negative electrode active material particles well to each other and also to adhere the negative electrode active material well to the current collector. The binder may be an insoluble binder, a water-soluble binder, or a combination thereof.
[0092] The above-mentioned non-aqueous binder may include polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, a polymer containing ethylene oxide, an ethylene propylene copolymer, polystyrene, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or a combination thereof.
[0093] The water-soluble binder may be a rubber-based binder or a polymer resin binder. The rubber-based binder may be selected from styrene-butadiene rubber, acrylated styrene-butadiene rubber, acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber, and combinations thereof. The polymer resin binder may be selected from polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, ethylene propylene diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenol resin, epoxy resin, polyvinyl alcohol, and combinations thereof.
[0094] When a water-soluble binder is used as the negative electrode binder, a cellulose-based compound capable of imparting viscosity as a type of thickener may be further included. The cellulose-based compound may be a mixture of one or more of carboxymethyl cellulose, hydroxypropylmethyl cellulose, methyl cellulose, or an alkali metal salt thereof. The alkali metal may be Na, K, or Li. The amount of the thickener used may be 0.1 to 3 parts by weight based on 100 parts by weight of the negative electrode active material.
[0095] The above conductive material is used to provide conductivity to the electrode, and in the battery to be formed, any material that does not cause a chemical change and is electronically conductive can be used. Examples of conductive materials that can be used include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, carbon nanofiber, and carbon nanotube; metal-based materials including copper, nickel, aluminum, silver, etc. and in the form of metal powder or metal fiber; conductive polymers such as polyphenylene derivatives; or conductive materials including mixtures thereof.
[0096] The negative electrode current collector may be selected from the group consisting of copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.
[0097] As another example, the negative electrode for an all-solid-state secondary battery may be a precipitation-type negative electrode. The precipitation-type negative electrode may refer to a negative electrode that does not include a negative electrode active material when the battery is assembled, but in which lithium metal or the like is precipitated or deposited on the negative electrode when the battery is charged, and this acts as a negative electrode active material.
[0098] Fig. 2 is a schematic cross-sectional view of an all-solid-state secondary battery including a precipitation-type negative electrode. Referring to Fig. 2, the precipitation-type negative electrode (400') may include a current collector (401) and a negative electrode coating layer (405) positioned on the current collector. An all-solid-state secondary battery including such a precipitation-type negative electrode (400') starts initial charging in a state in which no negative electrode active material is present, and during charging, high-density lithium metal is precipitated or deposited between the current collector (401) and the negative electrode coating layer (405) or on the negative electrode coating layer (405) to form a lithium metal layer (404), which may function as a negative electrode active material. Accordingly, in an all-solid-state secondary battery that has been charged more than once, the precipitation-type negative electrode (400') may include, for example, a current collector (401), a lithium metal layer (404) positioned on the current collector, and a negative electrode coating layer (405) positioned on the metal layer. The lithium metal layer (404) refers to a layer in which lithium metal or the like is precipitated during the charging process of the battery, and may be referred to as a metal layer, a lithium layer, a lithium deposition layer, or a negative electrode active material layer.
[0099] In this case, the aforementioned area or first solid electrolyte layer can be said to be a surface in contact with the cathode coating layer (405).
[0100] The above cathode coating layer (405) may be referred to as a lithium electrodeposition induction layer or a cathode catalyst layer, and may include a metal, carbon material, or a combination thereof that acts as a catalyst.
[0101] The metal may be a lithium-philic metal, and may include, for example, gold, platinum, palladium, silicon, silver, aluminum, bismuth, tin, zinc, or a combination thereof, and may be composed of one type of these or may be composed of several types of alloys. When the metal is present in the form of particles, the average particle diameter (D50) thereof may be about 4 μm or less, and may be, for example, 10 nm to 4 μm.
[0102] The carbon material may be, for example, crystalline carbon, amorphous carbon, or a combination thereof. The crystalline carbon may be, for example, natural graphite, artificial graphite, mesophase carbon microbeads, or a combination thereof. The amorphous carbon may be, for example, carbon black, activated carbon, acetylene black, Denka black, Ketjen black, or a combination thereof.
[0103] When the above-described negative electrode coating layer (405) includes both the metal and the carbon material, the mixing ratio of the metal and the carbon material may be, for example, a weight ratio of 1:10 to 2:1. In this case, the precipitation of lithium metal can be effectively promoted and the characteristics of the all-solid-state secondary battery can be improved. The above-described negative electrode coating layer (405) may include, for example, a carbon material supported with a catalytic metal, or may include a mixture of metal particles and carbon material particles.
[0104] The above-described cathode coating layer (405) may include, for example, the above-described lithium-philic metal and amorphous carbon, in which case the precipitation of the lithium metal may be effectively promoted. As a specific example, the cathode coating layer (405) may include a composite in which a lithium-philic metal is supported on amorphous carbon.
[0105] The above cathode coating layer (405) may further include a binder, and the binder may be, for example, a conductive binder. In addition, the above cathode coating layer (405) may further include general additives such as fillers, dispersants, and ionic conductive agents.
[0106] The thickness of the cathode coating layer (405) may be, for example, 100 nm to 20 ㎛, or 500 nm to 10 ㎛, or 1 ㎛ to 5 ㎛.
[0107] The above-described precipitated negative electrode (400') may further include, for example, a thin film on the surface of the current collector, i.e., between the current collector and the negative electrode coating layer. The thin film may include an element capable of forming an alloy with lithium. The element capable of forming an alloy with lithium may be, for example, gold, silver, zinc, tin, indium, silicon, aluminum, bismuth, etc., and may be composed of one type thereof or may be composed of multiple types of alloys. The thin film may further flatten the precipitated form of the lithium metal layer (404) and further improve the characteristics of the all-solid-state secondary battery. The thin film may be formed by, for example, a vacuum deposition method, a sputtering method, a plating method, etc. The thickness of the thin film may be, for example, 1 nm to 500 nm.
[0108] The lithium metal layer (404) may include lithium metal or a lithium alloy. The lithium alloy may be, for example, a Li-Al alloy, a Li-Sn alloy, a Li-In alloy, a Li-Ag alloy, a Li-Au alloy, a Li-Zn alloy, a Li-Ge alloy, or a Li-Si alloy.
[0109] The thickness of the lithium metal layer (404) may be 1 μm to 500 μm, 1 μm to 200 μm, 1 μm to 100 μm, or 1 μm to 50 μm. If the thickness of the lithium metal layer (404) is too thin, it may be difficult to perform the role of a lithium storage, and if it is too thick, the battery volume may increase and performance may deteriorate.
[0110] When such a precipitation-type cathode is applied, the cathode coating layer (405) can play a role in protecting the lithium metal layer (404) and suppressing the precipitation growth of lithium deadlight. Accordingly, short-circuiting and capacity reduction of the all-solid-state battery can be suppressed, and the life characteristics can be improved.
[0111] anode
[0112] In one embodiment, the device comprises a current collector and a positive electrode active material layer positioned on the current collector, wherein the positive electrode active material layer comprises a positive electrode active material and a solid electrolyte, and may optionally comprise a binder and / or a conductive material. In this case, the positive electrode active material layer may comprise the aforementioned solid electrolyte.
[0113] positive electrode active material
[0114] The above-mentioned positive electrode active material can be applied without limitation as long as it is generally used in all-solid-state secondary batteries. For example, the above-mentioned positive electrode active material may be a compound capable of reversible intercalation and deintercalation of lithium, and may include a compound represented by any one of the following chemical formulas.
[0115] Li a A 1-b X b D2(0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5);
[0116] Li a A 1-b X b O 2-c D c (0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05);
[0117] Li a E 1-b X b O 2-c D c (0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05);
[0118] Li a E 2-b X b O 4-c D c (0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05);
[0119] Li a Ni 1-b-c Co b X c D α(0.90 ≤ a ≤1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.5, 0 <α ≤ 2);
[0120] Li a Ni 1-b-c Co b X c O 2-α T α (0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2);
[0121] Li a Ni 1-b-c Co b X c O 2-α T2(0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2);
[0122] Li a Ni 1-b-c Mr b X c D α (0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2);
[0123] Li a Ni 1-b-c Mr b X c O 2-α T α (0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2);
[0124] Li a Ni 1-b-c Mr b X c O 2-α T2(0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2);
[0125] Li a Ni b HAVE BEEN c G d O2(0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0.001 ≤ d ≤ 0.1);
[0126] The a Nor b Co c Mn d G e O2(0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤0.5, 0.001 ≤ e ≤ 0.1);
[0127] The a NiG b O2(0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1);
[0128] The a CoG b O2(0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1);
[0129] The a Mn 1-b G b O2(0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1);
[0130] The a Mn2G b O4(0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1);
[0131] The a Mn 1-g G g PO4(0.90 ≤ a ≤ 1.8, 0 ≤ g ≤ 0.5);
[0132] QO2; QS2; LiQS2;
[0133] V2O5; LiV2O5;
[0134] LiZO2;
[0135] LiNiVO4;
[0136] The (3-f) J2(PO4)3(0 ≤ f ≤ 2);
[0137] The (3-f) Fe2(PO4)3(0 ≤ f ≤ 2);
[0138] The a FePO4(0.90 ≤ a ≤ 1.8).
[0139] In the above chemical formulas, A is selected from the group consisting of Ni, Co, Mn, and combinations thereof; X is selected from the group consisting of Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, rare earth elements, and combinations thereof; D is selected from the group consisting of O, F, S, P, and combinations thereof; E is selected from the group consisting of Co, Mn, and combinations thereof; T is selected from the group consisting of F, S, P, and combinations thereof; G is selected from the group consisting of Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, and combinations thereof; Q is selected from the group consisting of Ti, Mo, Mn, and combinations thereof; Z is selected from the group consisting of Cr, V, Fe, Sc, Y, and combinations thereof; J is selected from the group consisting of V, Cr, Mn, Co, Ni, Cu, and combinations thereof.
[0140] The above-mentioned positive electrode active material may be, for example, lithium cobalt oxide (LCO), lithium nickel oxide (LNO), lithium nickel cobalt oxide (NC), lithium nickel cobalt aluminum oxide (NCA), lithium nickel cobalt manganese oxide (NCM), lithium nickel manganese oxide (NM), lithium manganese oxide (LMO), or lithium iron phosphate (LFP).
[0141] The positive electrode active material may include, for example, a lithium nickel-based oxide represented by the following chemical formula 11, a lithium cobalt-based oxide represented by the following chemical formula 12, a lithium iron phosphate-based compound represented by the following chemical formula 13, a cobalt-free lithium nickel-manganese-based oxide represented by the following chemical formula 14, or a combination thereof.
[0142] [Chemical Formula 11]
[0143] Li a1 Ni x1 M 1 y1 M 2 z1 O 2-b1 Xb1
[0144] In the above chemical formula 11, 0.9≤a1≤1.8, 0.3≤x1≤1, 0≤y1≤0.7, 0≤z1≤0.7, 0.9≤x1+y1+z1≤1.1, and 0≤b1≤0.1, and M 1 and M 2 are each independently one or more elements selected from the group consisting of Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sn, Sr, Ti, V, W, and Zr, and X is one or more elements selected from the group consisting of F, P, and S.
[0145] In the above chemical formula 1, 0.6≤x1≤1, 0≤y1≤0.4, and 0≤z1≤0.4, or 0.8≤x1≤1, 0≤y1≤0.2, and 0≤z1≤0.2.
[0146] [Chemical Formula 12]
[0147] Li a2 Co x2 M 3 y2 O 2-b2 X b2
[0148] In the above chemical formula 12, 0.9≤a2≤1.8, 0.7≤x2≤1, 0≤y2≤0.3, 0.9≤x2+y2≤1.1, and 0≤b2≤0.1, and M 3 is one or more elements selected from the group consisting of Al, B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mn, Mo, Ni, Se, Si, Sn, Sr, Ti, V, W, Y, Zn and Zr, and X is one or more elements selected from the group consisting of F, P and S.
[0149] [Chemical Formula 13]
[0150] Li a3 Fe x3 M 4 y3 PO 4-b3 X b3
[0151] In the above chemical formula 13, 0.9≤a3≤1.8, 0.6≤x3≤1, 0≤y3≤0.4, and 0≤b3≤0.1, and M 4 is one or more elements selected from the group consisting of Al, B, Ba, Ca, Ce, Co, Cr, Cu, Mg, Mn, Mo, Ni, Se, Si, Sn, Sr, Ti, V, W, Y, Zn and Zr, and X is one or more elements selected from the group consisting of F, P and S.
[0152] [Chemical Formula 14]
[0153] Li a4 Ni x4 Mn y4 M 5 z4 O 2-b4 X b4
[0154] In the above chemical formula 14, 0.9≤a2≤1.8, 0.8≤x4<1, 0 <y4≤0.2, 0≤z4≤0.2, 0.9≤x4+y4+z4≤1.1, 및 0≤b4≤0.1이고 M 5 is one or more elements selected from the group consisting of Al, B, Ba, Ca, Ce, Cr, Fe, Mg, Mo, Nb, Si, Sn, Sr, Ti, V, W, and Zr, and X is one or more elements selected from the group consisting of F, P, and S.
[0155] The average particle diameter (D50) of the positive electrode active material may be 1 μm to 25 μm, for example, 3 μm to 25 μm, 1 μm to 20 μm, 1 μm to 18 μm, 3 μm to 15 μm, or 5 μm to 15 μm. For example, the positive electrode active material may include small particles having an average particle diameter (D50) of 1 μm to 9 μm and large particles having an average particle diameter (D50) of 10 μm to 25 μm. A positive electrode active material having such a particle diameter range can be harmoniously mixed with other components within a positive electrode active material layer and can realize high capacity and high energy density. Here, the average particle diameter may be obtained by selecting 20 or so random particles from a scanning electron microscope image of the positive electrode active material, measuring their particle diameters (diameter, major axis, or major axis length), obtaining a particle size distribution, and then taking the diameter (D50) of particles having a cumulative volume of 50% by volume from the particle size distribution as the average particle diameter.
[0156] The above-mentioned positive electrode active material may be in the form of a secondary particle formed by agglomeration of a plurality of primary particles, or may be in the form of a single particle. In addition, the above-mentioned positive electrode active material may be spherical or nearly spherical in shape, or may be polyhedral or irregular in shape.
[0157] Meanwhile, the positive electrode active material may include a buffer layer on the particle surface. The buffer layer may be expressed as a coating layer, a protective layer, etc., and may play a role in lowering the interfacial resistance between the positive electrode active material and the sulfide-based solid electrolyte particles. For example, the buffer layer may include a lithium-metal-oxide, wherein the metal may be one or more elements selected from the group consisting of Al, B, Ca, Ce, Cr, Fe, Mg, Mo, Nb, Si, Sn, Sr, Ta, V, W, and Zr. The lithium-metal-oxide is excellent in lowering the interfacial resistance between the positive electrode active material and the solid electrolyte particles while improving the performance of the positive electrode active material by facilitating the movement of lithium ions and electron conduction.
[0158] The positive electrode active material may be included in an amount of 55 wt% to 99 wt% based on 100 wt% of the positive electrode active material layer, for example, 65 wt% to 95 wt%, or 75 wt% to 91 wt%.
[0159] bookbinder
[0160] The above binder serves to adhere the positive electrode active material particles well to each other and also to adhere the positive electrode active material well to the current collector, and representative examples thereof include, but are not limited to, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc.
[0161] The content of the binder in the positive electrode active material layer may be approximately 0.1 wt% to 5 wt% with respect to 100 wt% of the positive electrode active material layer.
[0162] Challenge
[0163] The above-described positive electrode active material layer may further include a conductive material. The conductive material is used to provide conductivity to the electrode, and any material that does not cause a chemical change and is electronically conductive in the battery to be constructed may be used. Examples of conductive materials that may be used include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, carbon nanofiber, carbon nanotube, etc.; metal-based materials containing copper, nickel, aluminum, silver, etc. in the form of metal powder or metal fiber; conductive polymers such as polyphenylene derivatives; or conductive materials including mixtures thereof.
[0164] The content of the conductive material in the positive electrode active material layer may be 0 wt% to 3 wt%, 0.01 wt% to 2 wt%, or 0.1 wt% to 1 wt% with respect to 100 wt% of the positive electrode active material layer.
[0165] With respect to 100 wt% of the above positive electrode active material layer, the solid electrolyte may be included in an amount of 0.1 wt% to 35 wt%, for example, 1 wt% to 35 wt%, 5 wt% to 30 wt%, 8 wt% to 25 wt%, or 10 wt% to 20 wt%.
[0166] In addition, in the positive electrode active material layer, 65 wt% to 99 wt% of the positive electrode active material and 1 wt% to 35 wt% of the solid electrolyte may be included based on the total weight of the positive electrode active material and the solid electrolyte, for example, 80 wt% to 90 wt% of the positive electrode active material and 10 wt% to 20 wt% of the solid electrolyte may be included. When the solid electrolyte is included in the positive electrode in such an amount, the efficiency and life characteristics of the all-solid-state battery can be improved without reducing the capacity.
[0167] Aluminum foil may be used as the positive electrode current collector, but is not limited thereto.
[0168] The above-mentioned all-solid-state secondary battery may be a unit cell having a structure of positive electrode / solid electrolyte layer / negative electrode, a bi-cell having a structure of negative electrode / solid electrolyte layer / positive electrode / solid electrolyte layer / negative electrode, or a laminated battery in which the structure of the unit cell is repeated.
[0169] The shape of the above-mentioned all-solid-state secondary battery is not particularly limited, and may be, for example, coin-shaped, button-shaped, sheet-shaped, stacked, cylindrical, flat, etc. In addition, the above-mentioned all-solid-state secondary battery can be applied to large-scale batteries used in electric vehicles, etc. For example, the above-mentioned all-solid-state secondary battery can be used in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs). In addition, it can be used in fields requiring a large amount of power storage, and for example, it can be used in electric bicycles or power tools, etc. In addition, the above-mentioned all-solid-state secondary battery can be used in various fields such as portable electronic devices.
[0170] Hereinafter, examples and comparative examples of the present invention are described. The following examples are merely examples of the present invention, and the present invention is not limited to the following examples.
[0171] Example 1
[0172] 1. Preparation of solid electrolyte
[0173] Argyrodite-type solid electrolyte particles (Li6PS5Cl, D50=3.5㎛) and polydimethylsiloxane (PDMS) having a number-average molecular weight of approximately 20,000 g / mol are prepared in a weight ratio of 1:1 and placed in an alumina crucible, respectively. Each alumina crucible is placed in a glass tube and heat-treated at 243°C for 1 hour in a vacuum atmosphere of 0.3 mmHg or less, thereby obtaining a solid electrolyte according to Example 1.
[0174] Example 2
[0175] A solid electrolyte is prepared in substantially the same manner as in Example 1, except that the solid electrolyte particles and PDMS are added in a weight ratio of 5:1.
[0176] Example 3
[0177] A solid electrolyte is prepared in substantially the same manner as in Example 1, except that the solid electrolyte particles and PDMS are added in a weight ratio of 10:1.
[0178] Example 4
[0179] A solid electrolyte is prepared in substantially the same manner as in Example 1, except that PDMS having a number average molecular weight of about 50,000 g / mol is used.
[0180] Example 5
[0181] A solid electrolyte is prepared in substantially the same manner as in Example 4, except that the solid electrolyte particles and PDMS are added in a weight ratio of 5:1.
[0182] Example 6
[0183] A solid electrolyte is prepared in substantially the same manner as in Example 4, except that the solid electrolyte particles and PDMS are added in a weight ratio of 10:1.
[0184] Example 7
[0185] A solid electrolyte is prepared in substantially the same manner as in Example 1, except that PDMS having a number average molecular weight of about 3,000 g / mol is used.
[0186] Example 8
[0187] A solid electrolyte is prepared in substantially the same manner as in Example 7, except that the solid electrolyte particles and PDMS are added in a weight ratio of 5:1.
[0188] Example 9
[0189] A solid electrolyte is prepared in substantially the same manner as in Example 7, except that the solid electrolyte particles and PDMS are added in a weight ratio of 10:1.
[0190] Example 10
[0191] The PDMS used in Example 1 is dissolved in n-heptane solvent, and then 1H,1H,2H,2H-perfluorodecyltriethoxysilane (PFDTES), a hydrophobic crosslinking agent, and dibutyltin dilaurate (DBTOL), an initiator, are added thereto, and stirred at room temperature for 12 hours. At this time, the weight ratio of PDMS / n-heptane / PFDTES / DBTOL is 1 / 10 / 0.4 / 0.005. The prepared solution is dried at room temperature for 12 hours and then dried at 120°C for 12 hours, thereby obtaining superhydrophobic F-PDMS containing a fluorine group.
[0192] A solid electrolyte is prepared in substantially the same manner as in Example 1, except that F-PDMS prepared by the above method is used instead of PDMS.
[0193] Example 11
[0194] Instead of argyrodite type solid electrolyte particles, halide type solid electrolyte particles (Li 2.5 In 0.5 Zr 0.5 A solid electrolyte is prepared in substantially the same manner as in Example 1, except that Cl6) is used.
[0195] Comparative Example 1
[0196] Uncoated argyrodite-type solid electrolyte particles (Li6PS5Cl, D50=3.5㎛) themselves are used as the solid electrolyte of Comparative Example 1.
[0197] Comparative Example 2
[0198] Uncoated halide-based solid electrolyte particles (Li 2.5 In 0.5 Zr 0.5Cl6) itself is used as a solid electrolyte in Comparative Example 2.
[0199] Evaluation Example 1: Cyro-TEM
[0200] Figure 3 is a cryogenic transmission electron microscope (Cyro-TEM) image of the solid electrolyte manufactured in Example 1. Referring to Figure 3, it can be confirmed that an amorphous coating layer several nm thick is formed on the surface of the solid electrolyte particles.
[0201] Evaluation Example 2: XPS
[0202] X-ray photoelectron spectroscopy (XPS) analysis was performed on the solid electrolyte of Comparative Example 1 before vapor deposition and the solid electrolyte of Example 1 after vapor deposition, respectively, and the results are shown in Fig. 4. For XPS, a K-Alpha+ equipment from Thermo Fisher Scientific was used, and an Al Kα light source was used under the conditions of 12 kV and 6 mA. To avoid exposure to the atmosphere, sampling was performed inside a glove box with an argon atmosphere, and the samples were moved to the measurement equipment without exposure to the atmosphere for analysis.
[0203] Referring to Fig. 4, it can be confirmed that bonds in the Si 2p region are formed as the hydrophobic polymer PDMS is vapor-deposited. Accordingly, it can be confirmed that the amorphous layer observed in Fig. 3 is a PDMS layer. For reference, the peak position of the Si-O bond 2p3 / 2 is 102 ± 0.1 eV, and the peak position of the Si-O bond 2p1 / 2 is 102.6 ± 0.1 eV.
[0204] Evaluation Example 3: TGA / DTA
[0205] Thermogravimetric analysis (TGA) was performed on the solid electrolyte of Comparative Example 1 and the solid electrolyte of Example 1, respectively, and the results are shown in Fig. 5. The TGA equipment used was a STA 449 F3 Jupiter Simultaneous Thermal Analyzer from NETZSCH. Approximately 5 mg of a solid electrolyte sample was placed on an alumina pan, and the weight change was measured while the temperature was increased from 30°C to 600°C at a rate of 10°C per minute under an argon atmosphere.
[0206] Referring to Figure 5, the difference in weight between Comparative Example 1 and Example 1 is analyzed to be approximately 4.0 wt%, which refers to the weight ratio occupied by the PDMS coating layer in the solid electrolyte of Example 1. That is, in Example 1, the coating layer is understood to be included at approximately 4.0 wt% with respect to 100 wt% of the solid electrolyte.
[0207] Evaluation Example 4: EIS
[0208] Electrochemical impedance spectroscopy (EIS) was performed on the solid electrolytes of Examples 1 to 9 and Comparative Example 1 before exposure to air and after being stored at a dew point of -50°C for 24 hours, and the results are shown in Table 1 below. Iviumstat from IVIUM Technologies Corp. was used as the EIS equipment, and analysis was performed from 1 Hz to 7 MHz under a voltage condition of 14.1 mV. A Nyquist plot was obtained through impedance analysis, from which the lithium ion conductivity of the solid electrolyte was calculated.
[0209] In Table 1 below, M n refers to the number-average molecular weight of PDMS, and the unit is g / mol. Ratio refers to the weight ratio of LiPSCl solid electrolyte particles to PDMS. σ pris is the ionic conductivity of the solid electrolyte before exposure to air, and σexpo is the ionic conductivity measured after exposing the solid electrolyte to the dew point of -50℃ for 24 hours, and the unit is mS / cm. σ expo / σ pris is σ pris σ for expo It is the value obtained by multiplying the ratio by 100, and the unit is %. The higher this value, the higher the atmospheric stability.
[0210] M n Ratioσ pris σ expo σ expo / σ pris Comparative Example 1--2.50.9136.1Example 1~20,0001:10.860.5058.8Example 25:12.11.047.6Example 310:12.41.145.8Example 4~50,0001:11.10.6660.0Example 55:11.90.8645.3Example 610:11.40.4834.3Example 7~3,0001:1---Example 85:11.30.5139.2Example 910:11.50.6644.0
[0211] Referring to Table 1 above, it can be confirmed that the solid electrolytes of the examples in which PDMS was vapor-deposited have improved atmospheric stability compared to Comparative Example 1. In particular, in Examples 1 to 3 using a polymer having a number-average molecular weight of ~20,000, the effect of improving atmospheric stability by the coating layer is greater, and in the case of Examples 1 and 4 in which the solid electrolyte particles and the hydrophobic polymer were introduced at a weight ratio of 1:1, the atmospheric stability effect is even higher. Separately, EIS was performed on the solid electrolytes of Comparative Example 1, Example 1, and Example 10 before exposure to air and after being left under harsh conditions with a dew point of -10°C for 24 hours, 48 hours, and 72 hours, to measure the change in ionic conductivity, and the results are shown in Table 2 below. The units of the values listed in the columns of Pristine, 24h, 48h, and 72h in Table 2 are S / cm, and 72h / pris is the ratio of 72h (ionic conductivity after 72 hours) to Pristine (ionic conductivity before exposure to air) multiplied by 100, and the unit is %, and a higher value is interpreted as a higher atmospheric stability.
[0212] Pristine24h48h72h72h / prisComparative Example 1(LPSCl)2.52 x 10 -3 2.39 x 10 -4 6.18 x 10 -6 3.78 x 10 -7 0.0150 Example 1 (PDMS-LPSCl) 2.27 x 10 -3 2.82 x 10 -4 5.64 x 10 -6 3.99 x 10 -7 0.0176 Example 10 (F-PDMS-LPSCl) 1.98 x 10 -3 2.74 x 10 -4 1.03 x 10 -5 4.29 x 10 -7 0.0217
[0213] Referring to Table 2, it can be seen that the atmospheric stability of Examples 1 and 10 is higher than that of Comparative Example 1. Separately, EIS was performed on the solid electrolytes of Comparative Example 2 and Example 11 using halide-based solid electrolyte particles before exposure to air and after leaving them at a dew point of -50°C for 24 hours to measure the change in ionic conductivity, and the results are shown in Table 3 below. σ pris and σ expo The unit is S / cm, and σ expo / σ pris is σ pris σ for expo It is the value obtained by multiplying the ratio by 100, and the unit is %. The higher this value, the higher the atmospheric stability is interpreted.
[0214] σ pris σ expo σ expo / σ pris Comparative Example 2 (LIZC) 1.4 x 10 -3 1.3 x 10 -4 9.3 Example 11 (PDMS-LIZC) 7.0 x 10 -4 1.8 x 10 -4 25.7
[0215] Referring to Table 3, it can be seen that the solid electrolyte of Example 11 has higher atmospheric stability than that of Comparative Example 2.
[0216] Although the preferred embodiments have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concepts defined in the following claims also fall within the scope of the present invention.
[0217] [Explanation of symbols]
[0218] 100: All-solid-state battery 200: Cathode
[0219] 201: Cathode current collector 203: Cathode active material layer
[0220] 300: Solid electrolyte layer 400: Cathode
[0221] 401: Negative current collector 403: Negative active material layer
[0222] 400': Precipitation type cathode 404: Lithium metal layer
[0223] 405: Cathode coating layer 500: Elastic layer
Claims
1. Comprising solid electrolyte particles and a coating layer positioned on the surface of the solid electrolyte particles, The above coating layer comprises a thermal decomposition product of a linear polysiloxane-based hydrophobic polymer, A solid electrolyte having a thickness of the coating layer of 1 nm to 50 nm.
2. In paragraph 1, The above coating layer is a solid electrolyte formed by a vapor deposition method.
3. In paragraph 1, A solid electrolyte having a thickness of the coating layer of 3 nm to 20 nm.
4. In paragraph 1, A solid electrolyte having a deviation in the thickness of the coating layer in one solid electrolyte particle of 30% or less.
5. In paragraph 1, A solid electrolyte having a standard deviation of the thickness of the coating layer in one solid electrolyte particle of 5 nm or less.
6. In paragraph 1, A solid electrolyte in which the coating layer is included in an amount of 1 to 5 wt% based on 100 wt% of the solid electrolyte.
7. In paragraph 1, The above linear polysiloxane-based hydrophobic polymer is a solid electrolyte comprising poly(dimethylsiloxane), poly(methylhydrosiloxane), poly(dimethylsiloxane-co-alkylmethylsiloxane), poly(dimethylsiloxane having a terminal vinyl group, poly(dimethylsiloxane having a terminal bis(hydroxylalkyl) group, poly(dimethylsiloxane having a terminal bis(3-aminopropyl) group), poly(dimethylsiloxane having a terminal hydroxyl group), or a combination thereof.
8. In paragraph 1, A solid electrolyte wherein the linear polysiloxane-based hydrophobic polymer contains a fluorine group.
9. In paragraph 8, A linear polysiloxane hydrophobic polymer containing a fluorine group is a solid electrolyte comprising 1H,1H,2H,2H-perfluorodecyltriethoxysilane, 1H,1H,2H,2H-perfluorododecyltrichlorosilane, 1H,1H,2H-perfluorooctyltridecoxysilane, or a combination thereof.
10. In paragraph 1, A solid electrolyte in which the linear polysiloxane-based hydrophobic polymer has a number average molecular weight of 3,000 g / mol to 50,000 g / mol.
11. In paragraph 1, The above coating layer is a non-crystalline solid electrolyte.
12. In paragraph 1, The above solid electrolyte particles are solid electrolytes including a sulfide-based solid electrolyte, an oxide-based solid electrolyte, a halide-based solid electrolyte, or a combination thereof.
13. In paragraph 1, A solid electrolyte having an average particle diameter (D50) of the above solid electrolyte particles of 0.1 ㎛ to 5.0 ㎛.
14. Solid electrolyte particles and linear polysiloxane hydrophobic polymers are introduced into a vacuum tube without contacting each other, A method for manufacturing a solid electrolyte, comprising heat-treating the vacuum tube to vapor-deposit the linear polysiloxane-based hydrophobic polymer on the surface of the solid electrolyte particles.
15. In paragraph 14, A method for producing a solid electrolyte, wherein the solid electrolyte particles and the linear polysiloxane-based hydrophobic polymer are introduced in a weight ratio of 95:5 to 40:
60.
16. In paragraph 1, A method for producing a solid electrolyte, wherein the solid electrolyte particles include a sulfide-based solid electrolyte, an oxide-based solid electrolyte, a halide-based solid electrolyte, or a combination thereof.
17. In paragraph 14, A method for producing a solid electrolyte, wherein the above heat treatment is performed at a temperature range of 150°C to 400°C.
18. In paragraph 14, A method for manufacturing a solid electrolyte, wherein the above heat treatment is performed for 0.5 to 6 hours.
19. An all-solid-state secondary battery comprising a solid electrolyte according to any one of claims 1 to 13.
Citation Information
Patent Citations
Method of preparing anode material for lithium secondary battery, anode material for lithium secondary battery prepared by the method, and secondary battery comprising the anode material
KR101103222B1
Solid electrolyte, manufacturing method thereof, and lithium battery employing the same
KR1020130000227A
Harmonic Suppression Matching Network and Power Amplifier including the same
KR1020230120441A