All-solid-state secondary battery

The integration of two-dimensional sulfide-based solid electrolytes in all-solid-state lithium batteries addresses interfacial resistance and dendrite growth issues, enhancing the performance and safety of lithium batteries by maintaining ion conduction and suppressing volume changes in the active material.

WO2024205088A1PCT designated stage expired Publication Date: 2024-10-03SAMSUNG SDI CO LTD

Patent Information

Application Number
PCT/KR2024/003351
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-03
Filing Date
2024-03-18
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional all-solid-state lithium batteries with solid electrolytes face challenges such as increased interfacial resistance, reduced ionic conductivity, and a higher risk of short circuits due to lithium dendrite growth, especially when using sulfide-based cathode active materials that undergo significant volume changes during charging and discharging.

Method used

Incorporating a two-dimensional sulfide-based solid electrolyte with a core/shell structure or irregular shape into the positive electrode active material layer to enhance ion conduction paths, reduce internal resistance, and suppress lithium dendrite growth, thereby improving cycle characteristics and safety.

Benefits of technology

The use of two-dimensional sulfide-based solid electrolytes effectively maintains ion conduction paths despite volume changes in the active material, reduces internal resistance, and suppresses lithium dendrite growth, leading to improved high-rate characteristics, output, and lifespan of the lithium batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024003351_03102024_PF_FP_ABST
    Figure KR2024003351_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This all-solid state secondary battery comprises a positive electrode layer, a negative electrode layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer, wherein: the positive electrode layer includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector; at least one of the positive electrode active material layer and the solid electrolyte layer comprises a first two-dimensional sulfide-based solid electrolyte; the negative electrode layer includes a negative electrode current collector and a first negative electrode active material layer disposed on at least one surface of the negative electrode current collector; and the initial charge capacity (B) of the first negative electrode active material layer is less than about 50% of the initial charge capacity (A) of the positive electrode active material layer.
Need to check novelty before this filing date? Find Prior Art

Description

All-solid-state secondary batteries

[0001] It's about all-solid-state secondary batteries.

[0002] Recently, there has been active development of batteries that offer increased energy density and safety. Lithium batteries are used in information technology, communication devices, and automobiles. Because automobiles are life-threatening, safety is paramount.

[0003] Lithium batteries containing liquid electrolytes contain flammable organic solvents. Lithium batteries containing liquid electrolytes have a high risk of overheating and fire in the event of a short circuit.

[0004] Solid electrolytes offer reduced risk of overheating and fire during short circuits compared to liquid electrolytes. Lithium batteries containing solid electrolytes can offer improved safety compared to those containing liquid electrolytes.

[0005] A lithium battery includes a cathode active material layer, and the cathode active material layer may include a conductive material to improve charge-discharge characteristics. The conductive material is, for example, a carbon-based conductive material. Carbon-based conductive materials have high electronic conductivity but low ionic conductivity. A solid electrolyte may be used to improve the ionic conductivity of the cathode active material layer. Conventional solid electrolytes have, for example, particle shapes with an aspect ratio of less than 2. Conventional solid electrolyte particles with an aspect ratio of less than 2 may have difficulty forming long-distance ionic conduction paths. In a lithium battery including conventional solid electrolyte particles with an aspect ratio of less than 2, the possibility of ion conduction path disconnection occurring during charge and discharge of the lithium battery increases. The lithium battery includes, for example, a sulfide-based cathode active material, and the sulfide-based cathode active material may undergo significant volume changes during charge and discharge. During charge and discharge of a lithium battery, conventional solid electrolyte particles having an aspect ratio of less than 2 may have difficulty suppressing the disconnection of ion conduction paths and increases in internal resistance due to volume changes in sulfide-based cathode active materials. Therefore, a method is required that can suppress the disconnection of ion conduction paths in a cathode active material layer due to volume changes in the cathode active material during charge and discharge of a lithium battery and suppress increases in internal resistance of the lithium battery.

[0006] Lithium batteries containing solid electrolytes may have relatively increased interfacial resistance and decreased ionic conductivity compared to lithium batteries containing liquid electrolytes. Therefore, lithium batteries containing solid electrolytes may have relatively poor high-rate characteristics and output characteristics compared to lithium batteries containing liquid electrolytes. Therefore, a method for increasing the high-rate characteristics and output characteristics of lithium batteries containing solid electrolytes by reducing interfacial resistance and increasing ionic conductivity in the lithium batteries containing solid electrolytes is required.

[0007] A lithium battery includes a solid electrolyte layer, and the solid electrolyte layer includes, for example, solid electrolyte particles having an aspect ratio of less than 2. Since the solid electrolyte layer includes solid electrolyte particles having an aspect ratio of less than 2, the length of an interfacial path between solid electrolyte particles formed in the thickness direction of the solid electrolyte layer may be similar to the thickness of the solid electrolyte layer. Accordingly, the path for lithium dendrites precipitated during the charge / discharge process of the lithium battery to pass through the solid electrolyte layer is shortened, and thus the possibility of a short circuit of the lithium battery due to the lithium dendrites may increase. Therefore, a method for more effectively suppressing the growth of lithium dendrites and more effectively suppressing a short circuit of a lithium battery is required.

[0008] One aspect is to provide a new all-solid-state secondary battery.

[0009] According to the implementation example

[0010] It comprises an anode layer; a cathode layer; and a solid electrolyte layer disposed between the anode layer and the cathode layer,

[0011] The above positive electrode layer includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface (e.g., one surface or both surfaces) of the positive electrode current collector,

[0012] At least one of the above cathode active material layer and the above solid electrolyte layer includes a first two-dimensional sulfide-based solid electrolyte,

[0013] The above negative electrode layer includes a negative electrode current collector and a first negative electrode active material layer disposed on at least one surface (e.g., one surface or both surfaces) of the negative electrode current collector,

[0014] An all-solid-state secondary battery is provided, wherein the initial charge capacity (B) of the first negative electrode active material layer is less than 50% of the initial charge capacity (A) of the positive electrode active material layer.

[0015] According to another implementation example

[0016] It comprises an anode layer; a cathode layer; and a solid electrolyte layer disposed between the anode layer and the cathode layer,

[0017] The above positive electrode layer includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface (e.g., one surface or both surfaces) of the positive electrode current collector,

[0018] At least one of the above cathode active material layer and the above solid electrolyte layer includes a first two-dimensional sulfide-based solid electrolyte,

[0019] An all-solid-state secondary battery is provided, wherein the negative electrode layer includes a negative electrode current collector and a first negative electrode active material layer disposed on at least one surface (e.g., one surface or both surfaces) of the negative electrode current collector.

[0020] According to another implementation example

[0021] It comprises an anode layer; a cathode layer; and a solid electrolyte layer disposed between the anode layer and the cathode layer,

[0022] The above positive electrode layer includes a positive electrode current collector and a positive electrode active material layer disposed on one or both sides of the positive electrode current collector,

[0023] An all-solid-state secondary battery is provided, wherein at least one of the positive electrode active material layer and the solid electrolyte layer includes a first two-dimensional sulfide-based solid electrolyte.

[0024] According to one aspect, it is possible to provide an all-solid-state secondary battery having a novel structure, in which short-circuiting is suppressed and cycle characteristics are improved.

[0025] Figure 1 is a schematic diagram of a two-dimensional sulfide-based solid electrolyte according to an exemplary embodiment.

[0026] Figure 2 is a schematic diagram of a two-dimensional sulfide-based solid electrolyte having a core / shell structure according to an exemplary embodiment.

[0027] Figure 3 is a cross-sectional view of a two-dimensional sulfide-based solid electrolyte having a core / shell structure according to an exemplary embodiment.

[0028] FIG. 4 is a cross-sectional view of a two-dimensional sulfide-based solid electrolyte having a core / intermediate layer / shell structure according to an exemplary embodiment.

[0029] FIGS. 5A to 5C are cross-sectional views of a cathode active material layer including a two-dimensional sulfide-based solid electrolyte according to an exemplary embodiment.

[0030] Figure 6 is a cross-sectional view of a solid electrolyte layer including a two-dimensional sulfide-based solid electrolyte according to an exemplary embodiment.

[0031] FIG. 7 is a cross-sectional view of a solid electrolyte layer including an irregularly shaped sulfide-based solid electrolyte according to an exemplary embodiment.

[0032] Figure 8 is a schematic diagram of a solid electrolyte layer including a two-dimensional sulfide-based solid electrolyte according to an exemplary embodiment.

[0033] Figure 9 is a schematic diagram of a solid electrolyte layer including an irregularly shaped sulfide-based solid electrolyte according to an exemplary embodiment.

[0034] Fig. 10 is a cross-sectional view of an all-solid-state secondary battery according to an exemplary embodiment.

[0035] Fig. 11 is a cross-sectional view of a bi-cell all-solid-state secondary battery according to an exemplary embodiment.

[0036] Fig. 12 is a cross-sectional view of an all-solid-state secondary battery according to an exemplary embodiment.

[0037] Fig. 13 is a cross-sectional view of an all-solid-state secondary battery according to an exemplary embodiment.

[0038] Fig. 14 is a cross-sectional view of a bi-cell all-solid-state secondary battery according to an exemplary embodiment.

[0039] Various embodiments are illustrated in the accompanying drawings. However, the present invention may be embodied in many different forms and should not be construed as limited to the embodiments described herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the present invention to those skilled in the art. Like reference numerals in the drawings indicate like elements.

[0040] When a component is referred to as being "on" another component, it can be understood that it is either directly on top of the other component or that other components may be intervening between them. Conversely, when a component is referred to as being "directly on" another component, no intervening components are present.

[0041] Although the terms "first," "second," "third," etc. may be used herein to describe various components, elements, regions, layers, and / or zones, these components, elements, regions, layers, and / or zones should not be limited by these terms. These terms are used only to distinguish one component, element, region, layer, or zone from another component, element, region, layer, or zone. Thus, a first component, element, region, layer, or zone described below may be referred to as a second component, element, region, layer, or zone without departing from the teachings of this specification.

[0042] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the invention. As used herein, the singular forms "a," "an," and "the" are intended to include the plural forms including "at least one," unless the content clearly dictates otherwise. "At least one" should not be construed as limiting to the singular. As used herein, the term "and / or" includes any and all combinations of one or more of the listed items. The terms "comprises" and / or "comprising" as used in the detailed description specify the presence of stated features, regions, integers, steps, operations, components, and / or ingredients, but do not preclude the presence or addition of one or more other features, regions, integers, steps, operations, components, ingredients, and / or groups thereof.

[0043] Spatially relative terms such as "below," "under," "bottom," "above," "above," and "top" may be used herein to readily describe the relationship of one component or feature to another. It will be understood that spatially relative terms are intended to encompass different orientations of the device when in use or operation in addition to the orientations depicted in the drawings. For example, if the device in the drawings were turned over, a component described as "below" or "below" another component or feature would then be oriented "above" the other component or feature. Thus, the exemplary term "below" can encompass both the above and below orientations. The device can be arranged in other orientations (rotated 90 degrees or otherwise rotated), and the spatially relative terms used herein can be interpreted accordingly.

[0044] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure pertains. Furthermore, it will be understood that terms defined in commonly used dictionaries should be interpreted to have a meaning consistent with their meaning within the context of the relevant art and the present disclosure, and not in an idealized or overly formal sense.

[0045] Exemplary embodiments are described herein with reference to cross-sectional drawings that are schematic representations of idealized embodiments. As such, variations from the shapes depicted are to be expected, for example, as a result of manufacturing techniques and / or tolerances. Therefore, the embodiments described herein should not be construed as limited to the specific shapes of regions as depicted herein, but should encompass variations in shapes resulting from, for example, manufacturing. For example, regions depicted or described as flat may typically have rough and / or non-linear features. Moreover, angles depicted as sharp may be rounded. Therefore, the regions depicted in the drawings are schematic in nature, and their shapes are not intended to depict the precise shapes of the regions, nor are they intended to limit the scope of the claims.

[0046] "Group" means a group in the periodic table of elements according to the International Union of Pure and Applied Chemistry ("IUPAC") Group 1-18 classification system.

[0047] In this specification, “aspect ratio” can be measured from, for example, scanning electron microscope (SEM), transmission electron microscope (TEM), and atomic force microscope (AFM) images.

[0048] In this specification, the “shape”, “structure”, “length”, “surface area” and / or “thickness” of the two-dimensional sulfide-based solid electrolyte can be measured from, for example, scanning electron microscope (SEM), transmission electron microscope (TEM) or atomic force microscope (AFM) images.

[0049] In this specification, the “thickness” and / or “diameter” of the core and shell of the positive electrode active material can be measured from, for example, scanning electron microscope (SEM), transmission electron microscope (TEM) or atomic force microscope (AFM) images.

[0050] In this specification, "particle size" refers to the average diameter when the particle is spherical, and the average major axis length when the particle is non-spherical. Particle size can be measured using a particle size analyzer (PSA). "Particle size" refers to the average particle diameter, for example. "Average particle size" refers to the median particle diameter, D50, for example.

[0051] D50 is the size of the particle corresponding to 50% of the cumulative volume, calculated from the particle side with a smaller particle size in the particle size distribution measured by laser diffraction.

[0052] D90 is the size of the particle corresponding to 90% of the cumulative volume, calculated from the particle side with a smaller particle size in the particle size distribution measured by laser diffraction.

[0053] D10 is the size of the particle corresponding to 10% of the cumulative volume, calculated from the particle side with a small particle size in the particle size distribution measured by laser diffraction.

[0054] In this disclosure, “metal” includes both metals and metalloids such as silicon and germanium, in their elemental or ionic states.

[0055] In this disclosure, “alloy” means a mixture of two or more metals.

[0056] In the present disclosure, “electrode active material” means an electrode material capable of undergoing lithiation and delithiation.

[0057] In the present disclosure, “positive electrode material” means a positive electrode material capable of undergoing lithiation and delithiation.

[0058] In the present disclosure, “negative electrode active material” means a negative electrode material capable of undergoing lithiation and delithiation.

[0059] In the present disclosure, “lithiation” and “lithiating” mean a process of adding lithium to an electrode active material.

[0060] In the present disclosure, “delithiation” and “delithiate” mean a process of removing lithium from an electrode active material.

[0061] In this disclosure, “charging” and “charging” mean a process of providing electrochemical energy to a battery.

[0062] In this disclosure, “discharging” and “discharging” mean the process of removing electrochemical energy from a battery.

[0063] In the present disclosure, “positive electrode” and “cathode” mean an electrode at which electrochemical reduction and lithiation occur during a discharge process.

[0064] In the present disclosure, “cathode” and “anode” mean electrodes where electrochemical oxidation and delithiation occur during a discharge process.

[0065] While specific implementations have been described, alternatives, modifications, variations, improvements, and substantial equivalents that are not currently anticipated or unforeseen may occur to the applicant or those skilled in the art. Accordingly, the appended claims, as filed and as amended, are intended to encompass all such alternatives, modifications, variations, improvements, and substantial equivalents.

[0066]

[0067] Hereinafter, an all-solid-state secondary battery according to exemplary implementation examples will be described in more detail.

[0068] [All-solid-state secondary battery]

[0069] According to one embodiment, an all-solid-state secondary battery includes a positive electrode layer; a negative electrode layer; and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer, wherein the positive electrode layer includes a positive electrode current collector and a positive electrode active material layer disposed on one or both surfaces of the positive electrode current collector, wherein at least one of the positive electrode active material layer and the solid electrolyte layer includes a first two-dimensional sulfide-based solid electrolyte, wherein the negative electrode layer includes a negative electrode current collector and a first negative electrode active material layer disposed on one surface of the negative electrode current collector, and wherein an initial charge capacity (B) of the first negative electrode active material layer is less than 50% of an initial charge capacity (A) of the positive electrode active material layer.

[0070] An all-solid-state secondary battery includes a cathode active material layer, and since the cathode active material layer includes a first two-dimensional sulfide-based solid electrolyte, a longer ion conduction path can be secured in the cathode active material layer. Accordingly, when charging and discharging the all-solid-state secondary battery, the ion conduction path disconnection due to volume change of the cathode active material in the cathode active material layer can be more effectively prevented. As a result, the initial efficiency, discharge capacity, high-rate characteristics, and / or cycle life characteristics of the all-solid-state secondary battery can be improved.

[0071] An all-solid-state secondary battery includes a cathode active material layer, and since the cathode active material layer includes a first two-dimensional sulfide-based solid electrolyte, the uniformity of the ion conduction path within the cathode active material layer can be improved. Accordingly, the pressure required during the manufacture of the all-solid-state secondary battery can be reduced. In other words, an all-solid-state secondary battery having an excellent ion conduction path can be realized even at a reduced pressure. In addition, the formation of local overvoltage within the cathode active material layer during the charge / discharge process of the all-solid-state secondary battery can be effectively prevented.

[0072] An all-solid-state secondary battery includes a cathode active material layer, and since the cathode active material layer includes a first two-dimensional sulfide-based solid electrolyte having a reduced specific surface area, moisture stability is increased, side reactions between the cathode active material and the sulfide-based solid electrolyte can be reduced, the interfacial resistance of the cathode active material layer can be reduced, and a decrease in ionic conductivity can be suppressed. Accordingly, the high-rate characteristics and output characteristics of the all-solid-state secondary battery can be improved.

[0073] An all-solid-state secondary battery includes a cathode active material layer, and since the cathode active material layer includes a first two-dimensional sulfide-based solid electrolyte, the volume change of the cathode active material during charge and discharge can be accommodated more effectively. A two-dimensional sulfide-based solid electrolyte can be arranged around the cathode active material in the cathode active material layer. The two-dimensional sulfide-based solid electrolyte can accommodate the volume change of the cathode active material during charge and discharge by distributing it over the entire area, and thus can accommodate the volume change of the cathode active material more effectively than, for example, a sulfide-based solid electrolyte in the form of spherical particles. Consequently, the disconnection between the cathode active material and the solid electrolyte due to the volume change of the cathode active material within the cathode active material layer can be suppressed, and the uniformity of the components within the cathode active material layer can be improved. Consequently, the cycle characteristics of the all-solid-state secondary battery can be improved.

[0074] Since the all-solid-state secondary battery includes a solid electrolyte layer, and the solid electrolyte layer includes a first two-dimensional sulfide-based solid electrolyte, the growth of lithium dendrites can be more effectively suppressed in the thickness direction of the solid electrolyte layer. Accordingly, the occurrence of short circuits, etc. due to the growth of lithium dendrites during charging and discharging of the all-solid-state secondary battery can be more effectively suppressed. As a result, the life characteristics of the all-solid-state secondary battery can be improved.

[0075] An all-solid-state secondary battery includes a solid electrolyte layer, and since the solid electrolyte layer includes a first two-dimensional sulfide-based solid electrolyte having an increased surface area, the possibility of pinhole formation on the surface of the solid electrolyte layer can be reduced during the manufacture of the solid electrolyte layer. Accordingly, the growth of lithium dendrites originating from the pinholes can be more effectively suppressed during charge and discharge of the all-solid-state secondary battery. As a result, the life characteristics of the all-solid-state secondary battery can be improved.

[0076]

[0077] Referring to FIGS. 1 to 13, an all-solid-state secondary battery (1) includes a positive electrode layer (10); a negative electrode layer (20); and a solid electrolyte layer (30) disposed between the positive electrode layer (10) and the negative electrode layer (20). The positive electrode layer (10) includes a positive electrode current collector (11) and a positive electrode active material layer (12) disposed on one or both surfaces of the positive electrode current collector. The positive electrode active material layer (12), the solid electrolyte layer (30), or a combination thereof includes a first two-dimensional sulfide-based solid electrolyte (100). The negative electrode layer (20) includes a negative electrode current collector (21) and a first negative electrode active material layer (22) disposed on one surface of the negative electrode current collector. An initial charge capacity (B) of the first negative electrode active material layer (22) is less than 50% of an initial charge capacity (A) of the positive electrode active material layer (12).

[0078]

[0079] [Anode layer]

[0080] [Anode layer: solid electrolyte]

[0081] The cathode active material layer (12) includes a first two-dimensional sulfide-based solid electrolyte.

[0082] Referring to FIGS. 1 to 4, the first two-dimensional sulfide-based solid electrolyte (100) is defined by a length (L) and a thickness (T). The length (L) of the first two-dimensional sulfide-based solid electrolyte (100) is the maximum value among the distances between the two ends of the first two-dimensional solid electrolyte (100) in a direction orthogonal to the thickness direction (y direction) of the first two-dimensional sulfide-based solid electrolyte (100). The thickness (T) of the first two-dimensional sulfide-based solid electrolyte (100) is the maximum value among the distances between the two ends of the first two-dimensional solid electrolyte (100) in the thickness direction (y direction) of the first two-dimensional sulfide-based solid electrolyte (100). Alternatively, the first two-dimensional sulfide-based solid electrolyte (100) includes a first surface (S1), a second surface (S2) facing the first surface (S1), and side surfaces (S3a, S3b, S3c, S3d) connecting the first surface (S1) and the second surface (S2), and is defined by the area of ​​the first surface (S1) or the second surface (S1) and the height of the side surfaces (S3a, S3b, S3c, S3d). The area of ​​the first surface (S1) or the second surface (S2) is, for example, the product of the maximum value and the minimum value of the distance between the two ends of the perimeter of the first surface (S1) or the second surface (S2). The height of the side surfaces (S3a, S3b, S3c, S3d) is the maximum value of the distance between the first surface (S1) and the second surface (S2). Alternatively, the area of ​​the first surface or the second surface is an integral of the area read from a scanning electron microscope plane view image in the thickness direction (y direction) of the first two-dimensional sulfide-based solid electrolyte (100). The height of the side is a maximum value of the height read from a scanning electron microscope side view image in the length direction (x direction or z direction) of the first two-dimensional sulfide-based solid electrolyte (100).

[0083] The aspect ratio of the length (L) and the thickness (T) of the first two-dimensional sulfide-based solid electrolyte (100) is, for example, 3 or more, 4 or more, 5 or more, 10 or more, or 20 or more. The aspect ratio of the length (L) and the thickness (T) of the first two-dimensional sulfide-based solid electrolyte (100) is, for example, 3 to 500, 3 to 400, 4 to 300, 5 to 200, or 10 to 200. Since the aspect ratio of the first two-dimensional sulfide-based solid electrolyte (100) has this range, the ion conduction path is extended in a lithium battery including the first two-dimensional sulfide-based solid electrolyte (100), and the volume change of the positive electrode active material during charge and discharge of the lithium battery can be accommodated more effectively, and the ion conduction path in the lithium battery can be maintained despite the volume change of the positive electrode active material. As a result, deterioration of the lithium battery can be suppressed and the cycle characteristics of the lithium battery can be improved.

[0084] The length (L) of the first two-dimensional sulfide-based solid electrolyte (100) may be, for example, 0.1 to 50 μm, 0.5 to 50 μm, 1 to 50 μm, 1 to 30 μm, 1 to 20 μm, or 1 to 10 μm. The thickness (T) of the first two-dimensional sulfide-based solid electrolyte (100) may be, for example, 10 nm to 30 μm, 10 nm to 20 μm, 10 nm to 10 μm, 10 nm to 5 μm, 10 nm to 1 μm, 10 nm to 500 nm, 10 nm to 300 nm, or 10 nm to 100 nm. Since the length and / or thickness of the first two-dimensional sulfide-based solid electrolyte (100) is within this range, the ion conduction path is extended within a lithium battery including the first two-dimensional sulfide-based solid electrolyte (100), and the volume change of the positive electrode active material during charge and discharge of the lithium battery can be accommodated more effectively, and the ion conduction path within the lithium battery can be maintained despite the volume change of the positive electrode active material. As a result, deterioration of the lithium battery can be suppressed, and the cycle characteristics of the lithium battery can be improved.

[0085] The first two-dimensional sulfide-based solid electrolyte (100) may include, for example, a plate structure, a flake structure, or a combination thereof, but is not necessarily limited to these forms, and any two-dimensional structure used in the relevant technical field may be used. Since the first two-dimensional sulfide-based solid electrolyte (100) has a plate structure, a flake structure, or the like, the ion conduction path is extended in a lithium battery including the first two-dimensional sulfide-based solid electrolyte (100), and the volume change of the positive electrode active material during charge and discharge of the lithium battery can be accommodated more effectively, and the ion conduction path in the lithium battery can be maintained despite the volume change of the positive electrode active material. As a result, deterioration of the lithium battery can be suppressed, and the cycle characteristics of the lithium battery can be improved.

[0086] The surface (S1, S2) of the first two-dimensional sulfide-based solid electrolyte (100) may have, for example, an irregular, circular, or polygonal shape. The shape of the surface (S1, S2) of the first two-dimensional sulfide-based solid electrolyte (100) is, for example, a shape determined by a plane view in the thickness direction (y direction) of the first two-dimensional sulfide-based solid electrolyte (100). The polygonal shape includes, but is not necessarily limited to, a triangle, a square, a pentagon, a hexagon, a heptagon, an octagon, a nonagon, or a decagon, and any shape that is used in the art and has a polygonal shape is possible.

[0087] Referring to FIGS. 2 to 4, the first two-dimensional sulfide-based solid electrolyte (100) may have, for example, a core (110) / shell (120) structure including a core (110) and a shell (120) disposed on the core (110). Since the first two-dimensional sulfide-based solid electrolyte (100) has a core (110) / shell (120) structure, the ion conduction path is extended within a lithium battery including the first two-dimensional sulfide-based solid electrolyte (100), and the volume change of the positive electrode active material during charge / discharge of the lithium battery can be accommodated more effectively, and the ion conduction path within the lithium battery can be maintained despite the volume change of the positive electrode active material. As a result, deterioration of the lithium battery can be suppressed, and the cycle characteristics of the lithium battery can be improved. In contrast, a simple mixture of a core (110) material and a shell (120) material is prone to agglomeration of the core (110) material and / or agglomeration of the shell (120) material, and thus does not provide an extended ion conduction path within a lithium battery. In addition, the volume change of the cathode active material during charge and discharge of the lithium battery cannot be accommodated more effectively, and the ion conduction path within the lithium battery may be interrupted by the volume change of the cathode active material. As a result, the deterioration of the lithium battery may increase and the cycle characteristics of the lithium battery may deteriorate. Therefore, the first two-dimensional sulfide-based solid electrolyte (100) having a core (110) / shell (120) structure is a composite in which the core (110) is covered by the shell (120), and is distinguished from a simple mixture of a core (110) material and a shell (120) material.

[0088] The core (110) may include, for example, a carbon-based material, a polymer material, a metal-containing inorganic material, a sulfide-based solid electrolyte, an oxide-based solid electrolyte, or a combination thereof. The core (110) may be any material capable of forming a two-dimensional structure.

[0089] Carbonaceous materials may include, but are not limited to, artificial graphite, natural graphite, carbon black (CB), acetylene black (AB), furnace black (FB), ketjen black (KB), graphene, graphene oxide, reduced graphene oxide, carbon nanobelt, carbon nanosheet, etc., and any carbonaceous material having a two-dimensional structure used in the relevant technical field may be used.

[0090] Polymeric materials include, for example, poly-2-vinylpyridine, polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene copolymer, polychlorotrifluoroethylene, perfluoroalkoxy copolymer, fluorinated cyclic ethers, polyethylene oxide diacrylate, polyethylene oxide dimethacrylate, polypropylene oxide diacrylate, polypropylene oxide dimethacrylate, polymethylene oxide diacrylate, polymethylene oxide dimethacrylate, polyalkyldiol diacrylate, polyalkyldiol dimethacrylate, polydivinylbenzene, polyethers, polycarbonates, polyamides, polyesters, polyvinyl chloride, polyimides, polycarboxylic acids, polysulfonic acids, polyvinyl alcohol, polysulfone, polystyrene, polyethylene, polypropylene, poly(p-phenylene), polyacetylene, poly(p-phenylene vinylene), polyaniline, polypyrrole, Polythiophene, poly(2,5-ethylene vinylene), polyacene, and poly(naphthalene-2,6-diyl), polyethylene oxide, polypropylene oxide, polyvinylidene fluoride, copolymer of vinylidene fluoride and hexafluoropropylene, poly(vinylacetate), poly(vinyl butyral-co-vinyl alcohol-co-vinyl acetate), poly(methyl methacrylate-co-ethyl acrylate), polyacrylonitrile, polyvinyl chloride-co-vinyl acetate, poly(1-vinylpyrrolidone-co-vinyl acetate), polyvinylpyrrolidone, polyacrylates, polymethacrylates, polyurethanes, polyvinyl ethers, acrylonitrile-butadiene rubber, styrene-butadiene rubber, acrylonitrile-butadiene-styrene rubber, sulfonated styrene / ethylene-butylene A polymer obtained from at least one acrylate monomer selected from the group consisting of triblock copolymer, ethoxylated neopentyl glycol diacrylate, ethoxylated bisphenol A diacrylate, ethoxylated aliphatic urethane acrylate, ethoxylated alkylphenol acrylate and alkyl acrylate, polyvinyl alcohol, polyimide,The polymer material may be one or more selected from epoxy resins and acrylic resins, or a combination thereof, but is not necessarily limited thereto, and any polymer capable of forming a two-dimensional structure in the art may be used. The polymer material may additionally include a lithium salt. The polymer material may have a two-dimensional structure.

[0091] The metal-containing inorganic material includes, but is not limited to, SiO2, TiO2, Al2O3, AlN, SiC, BaTiO3, MOF (Metal Organic Framework), POSS (Polyhedral Oligomeric Silsesquioxanes), Li2CO3, Li3PO4, Li3N, Li3S4, Li2O, montmorillonite, or a combination thereof, and any metal-containing inorganic material capable of forming a two-dimensional structure in the art may be used. The metal-containing inorganic material may have a two-dimensional structure. The metal-containing inorganic material may have a two-dimensional nanostructure.

[0092] Sulfide-based solid electrolytes include, for example, Li2S-P2S5, Li2S-P2S5-LiX, where X is a halogen element, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n , m, n are positive numbers, Z is one of Ge, Zn or Ga, Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q , p, q are positive numbers, M is one of P, Si, Ge, B, Al, Ga In, Li 7-x PS 6-x Cl x , 0≤x≤2, Li 7-xPS 6-x Br x , 0≤x≤2, and Li 7-x PS 6-x I x , at least one selected from 0≤x≤2. The sulfide-based solid electrolyte is manufactured by processing starting materials such as Li2S, P2S5, etc. by a melting rapid cooling method or a mechanical milling method. In addition, heat treatment may be performed after the processing. The sulfide-based solid electrolyte may be amorphous, crystalline, or a mixed state thereof. In addition, the sulfide-based solid electrolyte may be, for example, one containing sulfur (S), phosphorus (P), and lithium (Li) as constituent elements among the above-described sulfide-based solid electrolyte materials. For example, the sulfide-based solid electrolyte may be a material containing Li2S-P2S5. When using a sulfide-based solid electrolyte material containing Li2S-P2S5, the mixing molar ratio of Li2S and P2S5 is, for example, in the range of Li2S: P2S5= 50:50 to 90:10. The sulfide-based solid electrolyte is Li 7-x PS 6-x Cl x , 0≤x≤2, Li 7-x PS 6-x Br x , 0≤x≤2, and Li 7-x PS 6-x I x , may be an argyrodite-type compound including at least one selected from 0≤x≤2. The sulfide-based solid electrolyte may include at least one selected from Li6PS5Cl, Li6PS5Br, and Li6PS5I. The sulfide-based solid electrolyte may have a two-dimensional structure.

[0093] Oxide solid electrolytes include, for example, Li 1+x+y Al x Ti 2-x Si y P 3-y O 12(0 <x<2, 0≤y<3), BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT)(0≤x<1, 0≤y<1), PB(Mg3Nb 2 / 3 )O3-PbTiO3(PMN-PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, Li3PO4, Li x Ti y (PO4)3(0 <x<2, 0<y<3), Li x Al y Ti z (PO4)3(0 <x<2, 0<y<1, 0<z<3), Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0≤x≤1 0≤y≤1), Li x La y TiO3(0 <x<2, 0<y<3), Li2O, LiOH, Li2CO3, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2, Li 3+x La3M2O 12 (M = Te, Nb, or Zr, 0≤x≤10), or a combination thereof. The oxide-based solid electrolyte is manufactured, for example, by a sintering method. The oxide-based solid electrolyte is, for example, Li7La3Zr2O 12 (LLZO) and Li 3+x La3Zr 2-a M a O 12 (M doped LLZO, M=Ga, W, Nb, Ta, or Al, 0 <a<2, 0≤x≤10) 중에서 선택된 가넷계(Garnet-type) 고체전해질이다. 산화물계 고체전해질은 이차원 구조를 가질 수 있다.

[0094] The core (110) can be used as a template of the first two-dimensional sulfide-based solid electrolyte (100). The core (110) can have an excellent elastic modulus. The elastic modulus of the core (110) can be, for example, 1 MPa or more, 10 MPa or more, or 100 MPa or more. The elastic modulus of the core (110) can be, for example, 1 MPa to 1 GPa, 10 MPa to 1 GPa, or 100 MPa to 1 GPa. When the core (110) has an elastic modulus in this range, the mechanical properties of the first two-dimensional sulfide-based solid electrolyte (100) can be further improved.

[0095] The shell (120) may include, for example, a sulfide-based solid electrolyte, an oxide-based solid electrolyte, or a coating material. The coating material may be disposed on part or all of the core (110). The coating material may, for example, impart water resistance, adhesive strength, etc. to the core (110).

[0096] A sulfide-based solid electrolyte and an oxide-based solid electrolyte can be selected from among the solid electrolytes included in the core (110).

[0097] The coating material is not particularly limited, and any material that provides the first two-dimensional sulfide-based solid electrolyte (100) with properties necessary for a lithium battery, such as water resistance and adhesion, may be used. The coating material may be, for example, a sulfide-based solid electrolyte that substantially does not contain cross-linked sulfur and Li2S. The coating material may be, for example, a composition containing only Li2S and a compound containing an element of Group 14 to Group 15 of the Periodic Table of Elements, such as P, Si, and Ge. In a composition containing only Li2S and P2S5, the content of Li2S may be 70% to 85%. In a composition containing only Li2S and SiS2, the content of Li2S may be 50% to 80%. In a composition containing only Li2S and GeS2, the content of Li2S may be 50% to 80%. The composition described above may not observe a cross-linked sulfur peak in the Raman spectrum, and may not observe a Li2S peak in the XRD spectrum. The amount of hydrogen sulfide generated may be reduced by the sulfide-based solid electrolyte having the mole fraction described above. The amount of hydrogen sulfide generated may be reduced by the sulfide-based solid electrolyte not including cross-linked sulfur and not including Li2S. The sulfide-based solid electrolyte may be a sulfide glass.

[0098] The coating material is, for example, yLi2S-(100-xy)P2S5.xP2O5(0 <x<25 and 67<y<80)의 조성을 가지는 결정화 유리(crystallized glass)를 포함하는 황화물게 고체전해질일 수 있다. 이러한 결정화 유리는 오로토(ortho) 조성을 가짐에 의하여 물에 대하여 향상된 안정성을 가지며 황화수소 발생량이 감소될 수 있다. 오르토(ortho)라는 것은 일반적으로, 같은 산화물을 수화해 얻어지는 옥소산(oxo acid) 중에서, 가장 수화도(hydration degree)가 높은 물건을 말한다. Li2S-P2S5계의 황화물계 고체전해질에서 P2S5에 가장 Li2S가 많이 부가하고 있는 결정 조성, 즉 Li3PS4가 오르토 조성에 해당한다. 75 Li2S - 25 P2S5에서 Li2S의 몰분율이 75 % 이므로, 오르토 조성을 가지므로 가교 유황을 실질적으로 포함하지 않을 수 있다. 가교 유황이란, 예를 들어 Li2S 및 P2S5가 반응해서 이루어지는 S3P-S-PS3중의 2개의 인 원자를 가교 하는 유황이다. 이러한 가교 유황은 물과 반응하기 쉽고, 황화수소가 발생하기 쉽다. 황화물계 고체전해질이 가교 유황을 실질적으로 함유하지 않는 것은, 예를 들어 라만 분광 스펙트럼의 측정에 의해 확인할 수 있다. 라만 분광 스펙트럼에 있어서, S3P-S-PS3의 피크는 통상 402 cm -1 It appears in the Raman spectrum of the sulfide-based solid electrolyte at 402 cm -1 The peak of PS4 may not be detected at all in the Raman spectroscopy spectrum of sulfide-based solid electrolytes. 3- Peak (417 cm) indicating -1 ) can be checked. .

[0099] The coating material may include, for example, a binder. The binder may be, but is not limited to, polyethylene (PE), polypropylene, polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), styrene-butadiene rubber (SBR), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-chlorotrifluoroethylene copolymer, ethylene-tetrafluoroethylene copolymer, polychlorotrifluoroethylene, vinylidene fluoride-pentafluoropropylene copolymer, propylene-tetrafluoroethylene copolymer, ethylene-chlorotrifluoroethylene copolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer, vinylidene fluoride-perfluoromethyl vinyl ether-tetrafluoroethylene copolymer, ethylene-acrylic acid copolymer, or a combination thereof, as long as it can be used as a binder in the art, it is not necessarily limited to these.

[0100] At least one of the core (110) and the shell (120) may include a sulfide-based solid electrolyte. By including at least one of the core (110) and the shell (120) a compound-based solid electrolyte, excellent ionic conductivity and mechanical properties can be provided simultaneously.

[0101] The core (110) may include, for example, a two-dimensional nanostructure. Since the core (110) includes a two-dimensional nanostructure, the shell (120) placed on the core (110) can easily have a two-dimensional structure.

[0102] The two-dimensional nanostructure may include, but is not necessarily limited to, graphene, graphene oxide, reduced graphene oxide, carbon nanobelts, carbon nanosheets, carbon nanoplates, carbon nanoflakes, SiO2, TiO2, Al2O3, AlN, SiC, BaTiO3, or combinations thereof, and any material having a two-dimensional nanostructure and used in the relevant technical field may be used.

[0103] Since the first two-dimensional sulfide-based solid electrolyte (100) includes such a two-dimensional nanostructure as a core (110), the ion conduction path is extended within a lithium battery including the first two-dimensional sulfide-based solid electrolyte (100), and the volume change of the positive electrode active material during charge and discharge of the lithium battery can be accommodated more effectively, and the ion conduction path within the lithium battery can be maintained despite the volume change of the positive electrode active material. As a result, the deterioration of the lithium battery can be further suppressed, and the cycle characteristics of the lithium battery can be further improved.

[0104] Referring to FIGS. 2 to 4, the ratio of the first thickness (T1) of the core (110) to the first thickness (T2) of the shell (120) may be, for example, 1:0.01 to 1:1000, 1:0.1 to 1:100, 1:0.1 to 1:10, 1:0.5 to 1:5, 1:1 to 1:4, 1:1 to 1:3, or 1:1 to 1:2.

[0105] The ratio of the first length (L1) of the core (110) to the second length (L2) of the shell (120) may be 1:1 to 1:10, 1:1.01:1:5, 1.01:1:2, 1:1.03 to 1:1.5, 1:1.05 to 1:1.3, 1:1.05 to 1:1.1.

[0106] Since the first two-dimensional sulfide-based solid electrolyte (100) has a core (110) and a shell (120) having a thickness ratio and / or a length ratio within this range, the ion conduction path is extended within a lithium battery including the first two-dimensional sulfide-based solid electrolyte (100), and the volume change of the positive electrode active material during charge and discharge of the lithium battery can be accommodated more effectively, and the ion conduction path within the lithium battery can be maintained despite the volume change of the positive electrode active material. As a result, the deterioration of the lithium battery can be further suppressed, and the cycle characteristics of the lithium battery can be further improved.

[0107] Although not shown in the drawing, the core (110) may have a multilayer structure. Since the core (110) has a multilayer structure, the shape, physical properties, etc. of the core (110) can be more diversely controlled. The core (110) may have, for example, a two-layer structure, a three-layer structure, or a four-layer structure. Each layer of the core (110) having a multilayer structure may include the same or different materials.

[0108] Although not shown in the drawing, the shell (120) may have a multilayer structure. Since the shell (120) has a multilayer structure, the shape, physical properties, etc. of the shell (120) can be more diversely controlled. The shell (120) may have, for example, a two-layer structure, a three-layer structure, or a four-layer structure. Each layer of the shell (120) having a multilayer structure may include the same or different materials.

[0109] Referring to FIG. 4, an interlayer (130) may be further included between the core (110) and the shell (120). By further including the interlayer (130) in the first two-dimensional sulfide-based solid electrolyte (100), the bonding strength of the core (110) and the shell (120) may be improved, and the structural stability of the core (110) and the shell (120) may be improved. The interlayer (130) may be omitted.

[0110] The intermediate layer (130) may have a third thickness (T3) and a third length (L3). The third length (L3) of the intermediate layer (130) may be, for example, greater than the first length (L1) of the core (110) and less than the second length (L2) of the shell (120). The third length (L3) of the intermediate layer (130) may be, for example, 101% to 150%, 101% to 120%, or 101% to 110% of the first length (L1) of the core (110). The third thickness (T3) of the intermediate layer (130) may be, for example, 1% to 50%, 1% to 20%, or 1% to 10% of the first thickness (T1) of the core (110). The material of the intermediate layer (130) can be selected from the material used for the core (110) and the material used for the shell (120). The material of the intermediate layer can be, for example, a polymer.

[0111] Referring to FIG. 5A, the positive electrode layer (10) includes a positive electrode current collector (11) and a positive electrode active material layer (12), and the positive electrode active material layer (12) includes a first region (12A) adjacent to the positive electrode current collector (11) and a second region (12B) adjacent to the solid electrolyte layer (30). For example, a first two-dimensional sulfide-based solid electrolyte (100) may be disposed in the first region (12A) and the first two-dimensional sulfide-based solid electrolyte (100) may be free in the second region (12B). The thickness of the first region (12A) may be 50% or less, 40% or less, 30% or less, or 20% or less of the total thickness of the positive electrode active material layer (12). The first two-dimensional sulfide-based solid electrolyte (100) may be uniformly distributed, for example, within the first region (12A). Alternatively, the first two-dimensional sulfide-based solid electrolyte (100) may have a concentration gradient that decreases in the first region (12A) from, for example, the positive electrode current collector (11) toward the solid electrolyte layer (30). Since the first two-dimensional sulfide-based solid electrolyte (100) is disposed in the first region (12A) and is absent in the second region (12B), a long-distance ion conduction path in the first region (12A) having an increased separation distance from the positive electrode layer is more easily formed, thereby allowing lithium ions to be more easily conducted into the positive electrode active material layer (12). Accordingly, an increase in internal resistance during charge and discharge of the lithium battery can be suppressed, and the cycle characteristics of the lithium battery can be further improved.

[0112] Referring to FIG. 5B, the positive electrode layer (10) includes a positive electrode current collector (11) and a positive electrode active material layer (12), and the positive electrode active material layer (12) includes a first region (12A) adjacent to the positive electrode current collector (11) and a second region (12B) adjacent to the solid electrolyte layer (30). For example, a first two-dimensional sulfide-based solid electrolyte (100) may be disposed in the second region (12B), and the first two-dimensional sulfide-based solid electrolyte (100) may be free in the first region (12A). The thickness of the second region (12B) may be 50% or less, 40% or less, 30% or less, or 20% or less of the total thickness of the positive electrode active material layer (12). The first two-dimensional sulfide-based solid electrolyte (100) may be uniformly distributed, for example, within the second region (12B). Alternatively, the first two-dimensional sulfide-based solid electrolyte (100) may have a concentration gradient that decreases in the second region (12B) from, for example, the solid electrolyte layer (30) toward the positive electrode current collector (11). By disposing the first two-dimensional sulfide-based solid electrolyte (100) in the second region (12B) adjacent to the solid electrolyte layer (30), the interfacial resistance between the electrolyte layer (30) and the positive electrode active material layer (12) is more effectively reduced, and lithium ions can be more easily conducted from the solid electrolyte layer (30) into the positive electrode active material layer (12). Accordingly, an increase in internal resistance during charge and discharge of the lithium battery can be suppressed, and the cycle characteristics of the lithium battery can be further improved.

[0113] Referring to FIG. 5c, the positive electrode layer (10) includes a positive electrode current collector (11) and a positive electrode active material layer (12), and the positive electrode active material layer (12) includes a first region (12A) adjacent to the positive electrode current collector and a second region (12B) adjacent to the solid electrolyte layer (30). For example, the first two-dimensional sulfide-based solid electrolyte (100) may be disposed in the first region (12A) and the second region (12B). By simultaneously disposing the first two-dimensional sulfide-based solid electrolyte (100) in the first region (12A) and the second region (12B), the ionic conductivity of the positive electrode active material layer (12) may be improved overall.

[0114] Referring to FIGS. 5A to 5C and FIGS. 10 to 13, the content of the first two-dimensional sulfide-based solid electrolyte (100) may be, for example, 1 to 50 wt%, 1 to 40 wt%, 5 to 40 wt%, 10 to 40 wt%, 15 to 40 wt%, 20 to 40 wt%, or 25 to 40 wt% of the total weight of the positive electrode active material layer (12). The content of the first two-dimensional sulfide-based solid electrolyte (100) may be, for example, 1 to 30 wt%, 1 to 25 wt%, 1 to 20 wt%, 1 to 10 wt%, or 1 to 5 wt% of the total weight of the positive electrode active material layer (12). Since the positive electrode active material layer (12) has the content of the first two-dimensional sulfide-based solid electrolyte (100) in this range, the ion conduction path is extended within the positive electrode active material layer (12) including the first two-dimensional sulfide-based solid electrolyte (100), and the volume change of the positive electrode active material during charge and discharge of the lithium battery can be accommodated more effectively, and the ion conduction path within the lithium battery can be maintained despite the volume change of the positive electrode active material. As a result, the deterioration of the lithium battery can be further suppressed, and the cycle characteristics of the lithium battery can be further improved. If the content of the first two-dimensional sulfide-based solid electrolyte (100) is excessively high, the filling between the first two-dimensional sulfide-based solid electrolytes (100) within the positive electrode active material layer (12) may be incomplete, which may increase the interfacial resistance.

[0115] The cathode active material layer (12) may further include an irregularly shaped sulfide-based solid electrolyte that is distinct from the first two-dimensional sulfide-based solid electrolyte (100). The aspect ratio of the irregularly shaped sulfide-based solid electrolyte may be less than 2, 1.5 or less, or 1.3 or less. The particle size of the irregularly shaped sulfide-based solid electrolyte may be, for example, 0.1 to 50 ㎛, 0.1 to 50 ㎛, 0.1 to 30 ㎛, 0.1 to 20 ㎛, 0.1 to 10 ㎛, 0.1 to 5 ㎛, or 0.1 to 3 ㎛. The weight ratio of the first two-dimensional sulfide-based solid electrolyte (100) and the amorphous sulfide-based solid electrolyte may be, for example, 1:99 to 99:1, 5:95 to 95:5, 10:90 to 90:10, 20:80 to 80:20, or 30:70 to 70:30. The weight ratio of the first two-dimensional sulfide-based solid electrolyte (100) and the amorphous sulfide-based solid electrolyte may be, for example, 1:99 to 50:50, 3:97 to 40:60, 5:95 to 30:70, 5:95 to 25:75, or 5:95 to 20:80. When the first two-dimensional sulfide-based solid electrolyte (100) and the amorphous sulfide-based solid electrolyte have a weight ratio within this range, the deterioration of the lithium battery can be further suppressed and the cycle characteristics of the lithium battery can be further improved.

[0116] The size of the solid electrolyte included in the positive electrode active material layer (12) may be smaller than the size of the solid electrolyte included in the solid electrolyte layer (30). For example, the D50 average particle diameter of the solid electrolyte included in the positive electrode active material layer (12) may be 90% or less, 80% or less, 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, or 20% or less of the D50 average particle diameter of the solid electrolyte included in the solid electrolyte layer (30). The D50 average particle diameter is, for example, a median particle diameter (D50). The median particle diameter (D50) is the size of particles corresponding to 50% cumulative volume, calculated from the side of particles having a small particle size in a size distribution of particles measured by, for example, a laser diffraction method. The particle diameter of the sulfide-based solid electrolyte can be measured by using, for example, a measuring device such as a laser diffraction method or a dynamic light scattering method. The particle size is measured, for example, using a laser scattering particle size distribution meter (e.g., Horiba LA-920), and is the median particle size (D50) when 50% of the small particles are accumulated in volume conversion. Alternatively, the particle size of a sulfide-based solid electrolyte can be measured from a scanning electron microscope (SEM) image or an optical microscope.

[0117] [Anode layer: cathode active material]

[0118] Referring to FIGS. 10 to 14, the positive electrode active material layer (12) includes, for example, a positive electrode active material.

[0119] The cathode active material included in the cathode active material layer (12) is a cathode active material capable of reversibly absorbing and desorbing lithium ions. The cathode active material includes, for example, an oxide-based cathode active material, a sulfide-based cathode active material, or a combination thereof.

[0120] The oxide-based cathode active material includes, for example, a lithium transition metal oxide, a metal oxide, or a combination thereof. The lithium transition metal oxide includes, for example, lithium cobalt oxide, lithium nickel oxide, lithium nickel cobalt oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt mangense oxide, lithium manganate, lithium iron phosphate, or a combination thereof. The lithium oxide includes, for example, iron oxide, vanadium oxide, or a combination thereof.

[0121] Sulfide-based cathode active materials include, for example, nickel sulfide, copper sulfide, Li2S, Li2S-containing complexes, or combinations thereof.

[0122] The oxide-based cathode active material may be, for example, one or more composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof. The oxide-based cathode active material may be, for example, Li. a A 1-b B' b D2 (in the above formula, 0.90 ≤ a ≤ 1, and 0 ≤ b ≤ 0.5); Li a E 1-b B' b O 2-c D c (In the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); LiE 2-b B' b O 4-c D c (In the above formula, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Lia Ni 1-b-c Co b B' c D α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Co b B' c O 2-α F' α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Co b B' c O2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Mn b B' c D α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Mn b B' c O 2-α F' α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B' c O2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni b E c G d O2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0.001 ≤ d ≤ 0.1); Li a Ni b Co c Mn d Ge O2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, 0.001 ≤ e ≤ 0.1); Li a NiG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a CoG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a MnG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a Mn2G b O4 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); LiV2O5; LiI'O2; LiNiVO4; Li (3-f) J2(PO4)3(0 ≤ f ≤ 2); Li (3-f) Fe2(PO4)3(0 ≤ f ≤ 2); may include a compound represented by any one of the chemical formulas of LiFePO4.

[0123] In the chemical formula representing the above-described compound, A is Ni, Co, Mn, or a combination thereof; B' is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F' is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I' is Cr, V, Fe, Sc, Y, or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof. It is also possible to use a compound having a coating layer added to the surface of the above-described compound, or it is also possible to use a mixture of the above-described compound and the compound having a coating layer added. The coating layer added to the surface of the above-mentioned compound includes a coating element compound of, for example, an oxide, a hydroxide, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element of the coating element. The compound forming the coating layer is amorphous or crystalline. The coating elements included in the coating layer are Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The method for forming the coating layer is selected within a range that does not adversely affect the physical properties of the positive electrode active material. The coating method includes, for example, spray coating and dipping. Since the specific coating method is well understood by those working in the relevant field, a detailed description thereof will be omitted.

[0124] The oxide-based cathode active material may include, for example, a lithium transition metal oxide represented by the following chemical formulas 1 to 8:

[0125] <Chemical Formula 1>

[0126] Li a Ni x Co y M z O2-b A b

[0127] In the above chemical formula 1,

[0128] 1.0≤a≤1.2, 0≤b≤0.2, 0.8≤x<1, 0≤y≤0.3, 0 <z≤0.3, 및 x+y+z=1이고,

[0129] M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B), or a combination thereof,

[0130] A is F, S, Cl, Br or a combination thereof,

[0131] <Chemical Formula 2>

[0132] LiNi x Co y Mn z O2

[0133] <Chemical Formula 3>

[0134] LiNi x Co y Al z O2

[0135] In the above chemical formulas 2 and 3, 0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2 및 x+y+z=1이며,

[0136] <Chemical Formula 4>

[0137] LiNi x Co y Mn z Al w O2

[0138] In the above chemical formula 4, 0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2, 0<w≤0.2, 및 x+y+z+w=1이며,

[0139] <Chemical Formula 5>

[0140] Li a Co x M y O 2-b Ab

[0141] In the above chemical formula 5,

[0142] 1.0≤a≤1.2, 0≤b≤0.2, 0.9≤x≤1, 0≤y≤0.1, and x+y=1,

[0143] M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B), or a combination thereof,

[0144] A is F, S, Cl, Br or a combination thereof,

[0145] <Chemical Formula 6>

[0146] Li a Ni x Mn y M' z O 2-b A b

[0147] In the above chemical formula 6,

[0148] 1.0≤a≤1.2, 0≤b≤0.2, 0 <x≤0.3, 0.5≤y<1, 0<z≤0.3, 및 x+y+z=1이고,

[0149] M' is cobalt (Co), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B) or a combination thereof,

[0150] A is F, S, Cl, Br or a combination thereof,

[0151] <Chemical Formula 7>

[0152] Li a M1 x M2 y PO 4-b X b

[0153] In the above chemical formula 7, 0.90≤a≤1.1, 0≤x≤0.9, 0≤y≤0.5, 0.9 <x+y<1.1, 0≤b≤2 이며,

[0154] M1 is chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr) or a combination thereof,

[0155] M2 is magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), zinc (Zn), boron (B), niobium (Nb), gallium (Ga), indium (In), molybdenum (Mo), tungsten (W), aluminum (Al), silicon (Si), chromium (Cr), vanadium (V), scandium (Sc), yttrium (Y) or a combination thereof, and X is O, F, S, P or a combination thereof.

[0156] <Chemical Formula 8>

[0157] Li a M3 z PO4

[0158] In the above chemical formula 8, 0.90≤a≤1.1, 0.9≤z≤1.1,

[0159] M3 is chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr), or a combination thereof.

[0160] The oxide-based cathode active material may be covered by a covering layer. The covering layer may be any material known as a covering layer for cathode active materials of all-solid-state secondary batteries. Examples of the covering layer include Li2O-ZrO2 (LZO).

[0161] The size of the oxide-based cathode active material may be, for example, 0.1 to 30 μm, 0.5 to 20 μm, or 1 to 15 μm. The oxide-based cathode active material may be, for example, a single-crystal particle or a polycrystalline particle.

[0162] The sulfide-based cathode active material may include, for example, a Li2S-containing composite. The Li2S-containing composite includes, for example, a composite of Li2S and carbon, a composite of Li2S, carbon, and a solid electrolyte, a composite of Li2S and a solid electrolyte, a composite of Li2S and a lithium salt, a composite of Li2S, a lithium salt, and carbon, a composite of Li2S and a metal carbide, a composite of Li2S, carbon, and a metal carbide, a composite of Li2S and a metal nitride, a composite of Li2S, carbon, and a metal nitride, or a combination thereof.

[0163] The Li2S and carbon complex comprises carbon. The carbon may be any material containing carbon atoms that is used as a conductive material in the art. The carbon may be, for example, crystalline carbon, amorphous carbon, or a combination thereof. The carbon may be, for example, a sintered product of a carbon precursor. The carbon may be, for example, a carbon nanostructure. The carbon nanostructure may be, for example, a one-dimensional carbon nanostructure, a two-dimensional carbon nanostructure, a three-dimensional carbon nanostructure, or a combination thereof. The carbon nanostructure may be, for example, a carbon nanotube, a carbon nanofiber, a carbon nanobelt, a carbon nanorod, graphene, graphene oxide (GO), reduced graphene oxide (rGO), graphene balls (GB), or a combination thereof. The carbon may be, for example, porous carbon or non-porous carbon. The porous carbon may include, for example, periodic and regular two-dimensional or three-dimensional pores. The porous carbon may be, for example, carbon black such as Ketjen black, acetylene black, Denka black, thermal black, channel black, etc.; graphite, activated carbon, or a combination thereof. The form of the carbon may be, for example, particle form, sheet form, flake form, etc., but is not limited thereto, and any method used as carbon in the art may be used. The method for preparing the composite of Li2S and carbon may be, for example, a dry method, a wet method, or a combination thereof, but is not limited thereto, and the method for preparing the composite of Li2S and carbon in the art may be, for example, milling, heat treatment, deposition, etc., but is not necessarily limited thereto, and any method used in the art may be used.

[0164] The composite of Li2S, carbon, and a solid electrolyte comprises carbon and a solid electrolyte. Carbon refers to the composite of Li2S and carbon described above. The solid electrolyte may be any solid electrolyte that is used as an ion-conducting material in the relevant technical field, for example, an amorphous solid electrolyte. The solid electrolyte is, for example, an inorganic solid electrolyte. The solid electrolyte is, for example, a crystalline solid electrolyte, an amorphous solid electrolyte, or a combination thereof. The solid electrolyte is, for example, a sulfide-based solid electrolyte, an oxide-based solid electrolyte, or a combination thereof. The sulfide-based solid electrolyte comprises, for example, Li, S, and P, and may optionally further comprise a halogen element. The sulfide-based solid electrolyte may be selected from among the sulfide-based solid electrolytes used in the solid electrolyte layer. The sulfide-based solid electrolyte may have a density of, for example, 1×10 -5 It can have an ionic conductivity of S / cm or more. Sulfide-based solid electrolytes include, for example, Li3PO4-Li2SO4, Li2S-P2S5, Li2S-P2S5-LiX, where X is a halogen element, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n , m, n are positive numbers, Z is one of Ge, Zn or Ga, Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q , p, q are positive numbers, M is one of P, Si, Ge, B, Al, Ga In, Li 7-x PS 6-x Cl x , 0≤x≤2, Li 7-x PS 6-x Br x , 0≤x≤2, and Li 7-x PS 6-x I x, may include one or more selected from 0≤x≤2. The oxide-based solid electrolyte includes, for example, Li, O, and a transition metal element, and may optionally further include other elements. The oxide-based solid electrolyte may include, for example, 1×10 at room temperature. -5 It may be a solid electrolyte having an ionic conductivity of S / cm or more. The oxide-based solid electrolyte may be selected from oxide-based solid electrolytes used in the solid electrolyte layer. The solid electrolyte may be, for example, a mixture of a sulfide-based solid electrolyte and a lithium salt. For example, it may be a mixture of Li3PO4-Li2SO4 and a binary lithium salt, or a mixture of Li3PO4-Li2SO4 and a ternary lithium salt.

[0165] The composite of Li2S and a solid electrolyte includes a solid electrolyte. The solid electrolyte refers to the composite of Li2S, carbon, and a solid electrolyte described above.

[0166] The complex of Li2S and a lithium salt comprises a lithium salt compound. The lithium salt compound does not contain, for example, a sulfur (S) atom. The lithium salt compound can be, for example, a binary compound composed of lithium and one element selected from Groups 13 to 17 of the Periodic Table of Elements. The binary compound can include, for example, one or more selected from LiF, LiCl, LiBr, LiI, LiH, Li2S, Li2O, Li2Se, Li2Te, Li3N, Li3P, Li3As, Li3Sb, LiI3, and LiB3. The lithium salt compound can be, for example, a ternary compound composed of lithium and two elements selected from Groups 13 to 17 of the Periodic Table of Elements. The ternary compound includes, for example, one or more selected from Li3OCl, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiAlO2, LiAlCl4, LiNO3, Li2CO3, LiBH4, Li2SO4, Li3BO3, Li3PO4, Li4NCl, Li5NCl2, and Li3BN2. The lithium salt compound is particularly one or more lithium halide compounds selected from LiF, LiCl, LiBr, and LiI. The complex of Li2S and a solid electrolyte includes a solid electrolyte. The solid electrolyte refers to the solid electrolyte used in the complex of Li2S, carbon, and a solid electrolyte described above. The complex of Li2S and the solid electrolyte includes, for example, a complex of Li2S and one or more lithium salts selected from LiF, LiCl, LiBr, LiI, LiH, Li2S, Li2O, Li2Se, Li2Te, Li3N, Li3P, Li3As, Li3Sb, LiI3 and LiB3.

[0167] The complex of Li2S and a lithium salt and carbon includes a lithium salt compound and carbon. Carbon refers to the complex of Li2S and carbon described above.

[0168] The composite of Li2S and metal carbide includes metal carbide. The metal carbide is, for example, a two-dimensional metal carbide. The two-dimensional metal carbide is, for example, MXene. The two-dimensional metal carbide is, for example, M n+1 C n T x (M is a transition metal, T is a terminal group, T is O, OH and / or F, n=1, 2, or 3, and x is the number of terminal groups) is expressed as 2D metal carbides, for example, Ti2CT x , (Ti 0.5 , Nb 0.5 )2CT x , Nb2CT x , V2CT x , Ti3C2T x , (V 0.5 , Cr 0.5 )3C2T x , Ti3CNT x , Ta4C3T x , Nb4C3T x or a combination thereof. The surface of the two-dimensional metal carbide is terminated with O, OH and / or F.

[0169] The complex of Li2S, carbon, and metal carbide includes carbon and metal carbide. Carbon refers to the complex of Li2S and carbon described above. Metal carbide refers to the complex of Li2S and metal carbide described above.

[0170] The complex of Li2S and metal nitride includes a metal nitride. The metal nitride is, for example, a two-dimensional metal nitride. The two-dimensional metal nitride is, for example, M n+1 N n T x (M is a transition metal, T is a terminal group, T is O, OH and / or F, n=1, 2, or 3, and x is the number of terminal groups) is expressed as The surface of the two-dimensional metal nitride is terminated with O, OH and / or F.

[0171] A complex of Li2S, carbon, and a metal nitride includes carbon and a metal nitride. Carbon refers to the complex of Li2S and carbon described above. Metal carbide refers to the complex of Li2S and a metal nitride described above.

[0172] The Li2S-containing composite may further include, for example, a second two-dimensional sulfide-based solid electrolyte (not shown). The Li2S-containing composite may be a composite of Li2S and the second two-dimensional sulfide-based solid electrolyte, or a composite of Li2S and the second two-dimensional sulfide-based solid electrolyte and the above-described carbon, solid electrolyte, lithium salt, metal carbide, or metal nitride.

[0173] When the Li2S-containing composite further includes a second two-dimensional sulfide-based solid electrolyte, the degradation of the lithium battery can be further suppressed and the cycle characteristics of the lithium battery can be further improved. The size of the second two-dimensional sulfide-based solid electrolyte can be smaller than the size of the first two-dimensional sulfide-based solid electrolyte (100). The length and / or thickness of the second two-dimensional sulfide-based solid electrolyte can be 50% or less, 40% or less, 30% or less, 20% or less, or 10% or less of the length and / or thickness of the first two-dimensional sulfide-based solid electrolyte (100), respectively. The length and / or thickness of the second two-dimensional sulfide-based solid electrolyte can be 0.1 to 50%, 0.5 to 40%, 1 to 30%, 1 to 20%, or 1 to 10% of the length and / or thickness of the first two-dimensional sulfide-based solid electrolyte (100), respectively. The second two-dimensional sulfide-based solid electrolyte may have, for example, the same shape as the first two-dimensional sulfide-based solid electrolyte (100) but a smaller size. The second two-dimensional sulfide-based solid electrolyte may be easily distributed within the Li2S-containing composite due to the reduced length and / or thickness. The second two-dimensional sulfide-based solid electrolyte may further suppress deterioration of the lithium battery and further improve cycle characteristics of the lithium battery due to the reduced length and / or thickness.

[0174] The size of the sulfide-based cathode active material can be, for example, 0.1 to 50 μm, 0.5 to 30 μm, 0.5 to 20 μm, or 1 to 10 μm. The size of Li2S can be, for example, 1 nm to 10 μm, 10 nm to 5 μm, 10 nm to 3 μm, or 10 nm to 1 μm. The size of the Li2S-containing composite can be, for example, 0.1 to 50 μm, 0.5 to 30 μm, 0.5 to 20 μm, or 1 to 10 μm.

[0175] The cathode active material may be, for example, a composite cathode active material including a core that absorbs and releases lithium and a shell disposed on the core.

[0176] The composite cathode active material includes, for example, a core that absorbs and releases lithium; and a shell arranged along the surface of the core; wherein the shell has the chemical formula M a O b(0<a≤3, 0<b<4, a가 1, 2, 또는 3 이면, b는 정수가 아님)로 표시되는 1종 이상의 제1 금속산화물; 및 그래핀을 포함하며, 상기 제1 금속산화물이 그래핀 메트릭스 내에 배치되며, 상기 M은 원소주기율표 2족 내지 13족, 제15족 및 16족 중에서 선택된 하나 이상의 금속이다. 리튬을 흡장 방출하는 코어는 예를 들어 상술한 Li2S 함유 복합체를 포함하며, Li2S 함유 복합체는 예를 들어 Li2S와 탄소의 복합체, Li2S와 탄소와 고체전해질의 복합체, Li2S와 고체전해질의 복합체, Li2S와 리튬염의 복합체, Li2S와 리튬염과 탄소의 복합체, Li2S와 금속카바이드의 복합체, Li2S와 탄소와 금속카바이드의 복합체, Li2S와 금속나이트라이드의 복합체, Li2S와 탄소와 금속나이트라이드의 복합체 또는 이들의 조합을 포함한다. 리튬을 흡장 방출하는 코어는 예를 들어 화학식 1 내지 8로 표시되는 리튬전이금속산화물을 포함할 수 있다. 리튬을 흡장 방출하는 코어는 예를 들어 Ni 함량 80mol% 이상의 리튬전이금속산화물을 포함할 수 있다. 리튬을 흡장 방출하는 코어 상에 예를 들어 제1 금속산화물 및 그래핀을 포함하는 쉘이 배치된다. 종래의 그래핀은 응집됨에 의하여 코어 상에 균일한 코팅이 어렵다. 이에 반해, 상기 복합양극활물질은 그래핀 메트릭스에 배치된 복수의 제1 금속산화물을 포함하는 복합체를 사용함에 의하여, 그래핀의 응집을 방지하면서 코어 상에 균일한 쉘이 배치된다. 따라서, 코어와 전해액의 접촉을 효과적으로 차단함에 의하여 코어와 전해질의 접촉에 의한 부반응을 방지한다. 그래핀을 포함하는 쉘(shell)은 유연성을 가지므로 충방전시 복합양극활물질의 부피 변화를 용이하게 수용함에 의하여 복합양극활물질 내부의 크랙(crack) 발생이 억제된다. 그래핀은 높은 전자전도성을 가지므로, 복합양극활물질과 전해질 사이의 계면 저항이 감소한다.Accordingly, the internal resistance of the lithium battery is maintained or reduced despite the introduction of a shell including graphene. In addition, since the first metal oxide has withstand voltage, deterioration of the Li2S-containing complex or lithium transition metal oxide included in the core can be prevented during charge / discharge at high voltage. Consequently, the cycle characteristics and high-temperature stability of the lithium battery including the composite cathode active material are improved. The shell may include, for example, one kind of first metal oxide or two or more different first metal oxides. The metal included in the first metal oxide may be, for example, one or more selected from Al, Nb, Mg, Sc, Ti, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn, Sb, and Se. The first metal oxide is, for example, Al2O. z (0 <z<3), NbO x (0 <x<2.5), MgO x (0 <x<1), Sc2O z (0 <z<3), TiO y (0 <y<2), ZrO y (0 <y<2), V2O z (0 <z<3), WO y (0 <y<2), MnO y (0 <y<2), Fe2O z (0 <z<3), Co3O w (0 <w<4), PdO x (0 <x<1), CuO x (0 <x<1), AgO x (0 <x<1), ZnO x (0 <x<1), Sb2O z (0 <z<3), 및 SeO y (0 <y<2) 중에서 선택된 하나 이상일 수 있다. 그래핀 메트릭스 내에 이러한 제1 금속산화물이 배치됨에 의하여 코어 상에 배치된 쉘의 균일성이 향상되고, 복합양극활물질의 내전압성이 더욱 향상된다. 예를 들어, 쉘은 제1 금속산화물로 Al2O x (0 <x<3)를 포함한다. 쉘은 화학식 M a Oc (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3이면, c는 정수임)로 표시되는 1종 이상의 제2 금속산화물을 더 포함할 수 있다. 상기 M은 원소주기율표 2족 내지 13족, 제15족 및 16족 중에서 선택된 하나 이상의 금속이다. 예를 들어, 제2 금속산화물은 상기 제1 금속산화물과 동일한 금속을 포함하며, 제2 금속산화물의 a 와 c의 비율인 c / a가 상기 제1 금속산화물의 a 와 b의 비율인 b / a에 비하여 더 큰 값을 가진다. 예를 들어, c / a > b / a. The second metal oxide is selected from, for example, Al2O3, NbO, NbO2, Nb2O5, MgO, Sc2O3, TiO2, ZrO2, V2O3, WO2, MnO2, Fe2O3, Co3O4, PdO, CuO, AgO, ZnO, Sb2O3, and SeO2. The first metal oxide is a reduction product of the second metal oxide. The first metal oxide is obtained by reducing part or all of the second metal oxide. Therefore, the first metal oxide has a lower oxygen content and a higher oxidation number of the metal than the second metal oxide. For example, the shell is the first metal oxide Al2O x(0<x<3) 및 제2 금속산화물인 Al2O3를 포함한다. 쉘의 두께는 예를 들어 1 nm 내지 5 um, 1 nm 내지 1 um, 1 nm 내지 500 nm, 1 nm 내지 200 nm, 1 nm 내지 100 nm, 1 nm 내지 90 nm, 1 nm 내지 80 nm, 1 nm 내지 70 nm, 1 nm 내지 60 nm, 1 nm 내지 50 nm, 1 nm 내지 40 nm, 1 nm 내지 30 nm, 1 nm 내지 20 nm, 또는 1 nm 내지 10 nm이다. 쉘이 이러한 범위의 두께를 가짐에 의하여 복합양극활물질이 포함하는 리튬전지의 내부 저항 증가가 억제된다. 복합체가 포함하는 제1 금속산화물 및 제2 금속산화물 중에서 선택된 하나 이상의 평균입경은 1 nm 내지 1 um, 1 nm 내지 500 nm, 1 nm 내지 200 nm, 1 nm 내지 100 nm, 1 nm 내지 70 nm, 1 nm 내지 50 nm, 1 nm 내지 30 nm, 3 nm 내지 30 nm, 3 nm 내지 25 nm, 5 nm 내지 25 nm, 5 nm 내지 20 nm, 또는 7 nm 내지 20 nm일 수 있다. 제1 금속산화물 및 / 또는 제2 금속산화물이 이러한 나노 범위의 입경을 가짐에 의하여 복합체의 그래핀 메트릭스 내에 보다 균일하게 분포될 수 있다. 따라서, 이러한 복합체가 응집 없이 코어 상에 균일하게 코팅되어 쉘을 형성할 수 있다. 또한, 제1 금속산화물 및 / 또는 제2 금속산화물이 이러한 범위의 입경을 가짐에 의하여 코어 상에 보다 균일하게 배치될 수 있다. 따라서, 코어 상에 제1 금속산화물 및 / 또는 제2 금속산화물이 균일하게 배치됨에 의하여 내전압 특성을 보다 효과적으로 발휘할 수 있다. 제1 금속산화물 및 제2 금속산화물의 평균 입경은 예를 들어 레이저 회절 방식이나 동적 광산란 방식의 측정 장치를 사용하여 측정할 수 있다. 다르게는, 제1 금속산화물 및 제2 금속산화물의 입경은 주사전자현미경 및 투과전자현미경으로부터 측정될 수 있다.

[0177] The shape of the positive electrode active material is, for example, a particle shape such as a sphere or an ellipse. The particle size of the positive electrode active material is not particularly limited and is within a range applicable to positive electrode active materials of a conventional all-solid-state secondary battery. The content of the positive electrode active material of the positive electrode layer (10) is also not particularly limited and is within a range applicable to positive electrode layers of a conventional all-solid-state secondary battery. The content of the positive electrode active material included in the positive electrode active material layer (12) may be, for example, 10 wt% to 99 wt%, 10 wt% to 90 wt%, 10 wt% to 80 wt%, 10 wt% to 70 wt%, or 10 wt% to 50 wt% of the total weight of the positive electrode active material layer (12).

[0178] [Anode layer: conductive material]

[0179] The cathode active material layer (12) may further include a conductive material. The conductive material may be, for example, a carbon-based conductive material, a metal-based conductive material, or a combination thereof. The carbon-based conductive material may be, for example, graphite, carbon black, acetylene black, Ketjen black, carbon fiber, or a combination thereof, but is not limited thereto, and any material used as a carbon-based conductive material in the art may be used. The metal-based conductive material may be, for example, metal powder, metal fiber, or a combination thereof, but is not limited thereto, and any material used as a metal-based conductive material in the art may be used. The content of the conductive material included in the cathode active material layer (12) may be, for example, 1 wt% to 30 wt%, 1 wt% to 20 wt%, or 1 wt% to 10 wt% of the total weight of the cathode active material layer (12).

[0180] [Anode layer: binder]

[0181] The positive electrode active material layer (12) may further include a binder. The binder may be, for example, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, etc., but is not limited thereto, and any binder used in the relevant technical field may be used. The binder content included in the positive electrode active material layer (12) may be, for example, 1 wt% to 10 wt% of the total weight of the positive electrode active material layer (12). The binder may be omitted.

[0182] [Anode layer: Other additives]

[0183] The cathode active material layer (12) may further include additives such as fillers, coating agents, dispersants, and ion conductive aids in addition to the cathode active material, solid electrolyte, binder, and conductive agent described above.

[0184] As fillers, coating agents, dispersants, ion conductivity aids, etc. that can be included in the positive electrode active material layer (12), known materials generally used in electrodes of all-solid-state secondary batteries can be used.

[0185] [Anode layer: Anode current collector]

[0186] The positive electrode collector (11) uses a plate or foil made of, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The positive electrode collector (11) may be omitted. The thickness of the positive electrode collector (11) is, for example, 1 µm to 100 µm, 1 µm to 50 µm, 5 µm to 25 µm, or 10 µm to 20 µm.

[0187] The cathode current collector (11) may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. The base film may be, for example, an insulator. Since the base film includes an insulating thermoplastic polymer, when a short circuit occurs, the base film softens or liquefies, thereby blocking battery operation and suppressing a rapid increase in current. The metal layer may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), or an alloy thereof. The metal layer can act as an electrochemical fuse and be cut off in case of overcurrent to prevent a short circuit. The limit current and the maximum current can be controlled by adjusting the thickness of the metal layer. The metal layer can be plated or deposited on the base film. As the thickness of the metal layer decreases, the limit current and / or the maximum current of the positive electrode current collector (11) decreases, thereby improving the stability of the lithium battery in case of a short circuit. A lead tab can be added on the metal layer for connection to the outside. The lead tab can be welded to the metal layer or the metal layer / base film laminate by ultrasonic welding, laser welding, spot welding, etc. During welding, the base film and / or the metal layer melt, so that the metal layer can be electrically connected to the lead tab. In order to strengthen the welding of the metal layer and the lead tab, a metal chip can be added between the metal layer and the lead tab.The metal piece may be a thin piece of the same material as the metal of the metal layer. The metal piece may be, for example, a metal foil, a metal mesh, etc. The metal piece may be, for example, aluminum foil, copper foil, SUS foil, etc. After the metal piece is placed on the metal layer, the lead tab may be welded to the metal piece / metal layer laminate or the metal piece / metal layer / base film laminate. During welding, the base film, the metal layer, and / or the metal piece may melt, so that the metal layer or the metal layer / metal piece laminate may be electrically connected to the lead tab. A metal chip and / or a lead tab may be added to a portion of the metal layer. The base film may have a thickness of, for example, 1 to 50 μm, 1.5 to 50 μm, 1.5 to 40 μm, or 1 to 30 μm. When the base film has a thickness in this range, the weight of the electrode assembly can be more effectively reduced. The melting point of the base film may be, for example, 100 to 300°C, 100 to 250°C or less, or 100 to 200°C. Since the base film has a melting point within this range, the base film can be melted and easily bonded to the lead tab during the welding process of the lead tab. To improve the adhesion between the base film and the metal layer, a surface treatment such as corona treatment may be performed on the base film. The thickness of the metal layer may be, for example, 0.01 to 3 μm, 0.1 to 3 μm, 0.1 to 2 μm, or 0.1 to μm. Since the metal layer has a thickness within this range, conductivity can be maintained while ensuring the stability of the electrode assembly. The thickness of the metal piece may be, for example, 2 to 10 μm, 2 to 7 μm, or 4 to 6 μm. Since the metal piece has a thickness within this range, the connection between the metal layer and the lead tab can be performed more easily. By having this structure, the positive electrode collector (11) can reduce the weight of the positive electrode and consequently improve the energy density of the positive electrode and lithium battery.

[0188] [Anode layer: inert member]

[0189] Referring to FIGS. 12 to 14, the positive electrode (10) includes a positive electrode current collector (11), a positive electrode active material layer (12) disposed on one side of the positive electrode current collector, and further includes an inactive member (40, 40a, 40b) disposed on one side of the positive electrode layer (10).

[0190] By including the inert member (40), cracking of the solid electrolyte layer (30) is prevented during the manufacture and / or charging and discharging of the all-solid-state secondary battery (1), and as a result, the cycle characteristics of the all-solid-state secondary battery (2) are improved. In the all-solid-state secondary battery (1) that does not include the inert member (40), when the manufacture and / or charging and discharging of the all-solid-state secondary battery (1) is performed, uneven pressure is applied to the solid electrolyte layer (30) in contact with the positive electrode (10), which causes cracking of the solid electrolyte layer (30), and the possibility of a short circuit occurring due to the growth of lithium metal through the cracking increases.

[0191] An inert member (40) is disposed along the side surface of the positive electrode layer (10) to surround the positive electrode layer. The inert member (40) surrounds, for example, part or all of the side surface of the positive electrode (10) and is in contact with the solid electrolyte layer (30). By the inert member (40) surrounding the side surface of the positive electrode (10) and being in contact with the solid electrolyte layer (30), cracks in the solid electrolyte layer (30) that occur due to a pressure difference during the pressing process in the solid electrolyte layer (30) that is not in contact with the positive electrode (20) can be effectively suppressed. The inert member (40) surrounds the side surface of the positive electrode (10) and is separated from the negative electrode (20), more specifically, the first negative electrode active material layer (22). The inert member (40) surrounds the side surface of the positive electrode (10), is in contact with the solid electrolyte layer (30), and is separated from the negative electrode (20). Accordingly, the possibility of a short circuit occurring due to physical contact between the positive electrode (10) and the first negative electrode active material layer (22) or due to overcharging of lithium, etc., is suppressed. Referring to FIG. 3, an inert member (40) is disposed on one side of the positive electrode active material layer (12) and simultaneously on one side of the positive electrode current collector (11), thereby more effectively suppressing the possibility of a short circuit occurring due to contact between the positive electrode current collector (11) and the negative electrode (20). Alternatively, referring to FIG. 4, the inert member (40) is disposed on one side of the positive electrode active material layer (12) and between the solid electrolyte layer (40) and the positive electrode current collector (11) facing the solid electrolyte layer (40). The inert member (40) is not disposed on one side of the positive electrode current collector (11). By placing an inert member (40) between the positive electrode collector (11) and the solid electrolyte layer (30), a short circuit caused by contact between the positive electrode collector (11) and the negative electrode (20) can be effectively prevented.

[0192] Although not shown in the drawing, some or all of the inert members (40, 40a, 40b) may be arranged spaced apart from the side surface of the positive electrode layer (10). By arranging some or all of the inert members (40, 40a, 40b) spaced apart from the side surface of the positive electrode layer (10), the manufacturing process of the all-solid-state secondary battery (1) may be facilitated and the manufacturing speed of the all-solid-state secondary battery (1) may be increased. By arranging some or all of the inert members (40, 40a, 40b) spaced apart from the side surface of the positive electrode layer (10), the volume change in the side surface direction of the positive electrode layer (10) during charge and discharge may be more effectively accommodated, thereby further improving the life characteristics of the all-solid-state secondary battery (1). The distance between the side of the inert member (40, 40a, 40b) and the anode layer (10) is independently, for example, 0.1 µm to 10 mm, 1 µm to 1 mm, 1 µm to 500 µm, 1 µm to 100 µm, 1 µm to 50 µm or 1 µm to 10 µm.

[0193] The inert member (40) may further include a position determining unit (not shown) configured to determine the position of the inert member (40) on the solid electrolyte layer (30). Since the inert member (40) includes the position determining unit, the position at which the inert member (40) is placed on the solid electrolyte layer (30) can be easily determined. As a result, the manufacturing speed of the all-solid-state secondary battery (1) can be increased and the ease of manufacturing can be improved.

[0194] Referring to FIGS. 13 and 14, the inert member (40) extends from one side of the positive electrode (30) to the end of the solid electrolyte layer (30). By extending the inert member (40) to the end of the solid electrolyte layer (30), cracks occurring at the end of the solid electrolyte layer (30) can be suppressed. The end of the solid electrolyte layer (30) is the outermost part that is in contact with the side of the solid electrolyte layer (30). The inert member (40) extends to the outermost part that is in contact with the side of the solid electrolyte layer (30). The inert member (40) is separated from the negative electrode layer (20), more specifically, from the first negative electrode active material layer (22). The inert member (40) extends to the end of the solid electrolyte layer (30), but does not contact the negative electrode layer (20). The inert member (40) fills a space extending from, for example, one side of the anode layer (30) to the end of the solid electrolyte layer (30).

[0195] The inert member (40) may be, for example, a gasket. By using a gasket as the inert member (40), cracks in the solid electrolyte layer (30) caused by a pressure difference during the pressing process can be effectively suppressed.

[0196] The inert member (40) has, for example, a single-layer structure. Alternatively, the inert member (40) may have a multi-layer structure. In the inert member (40) having a multi-layer structure, each layer may have a different composition. The inert member having a multi-layer structure may have, for example, a two-layer structure, a three-layer structure, a four-layer structure, or a five-layer structure. The inert member (40) having a multi-layer structure may include, for example, one or more adhesive layers and one or more support layers. The adhesive layer effectively prevents, for example, a separation between the positive electrode layer (10) and the solid electrolyte layer (30) due to a change in the volume of the positive electrode layer (10) that occurs during the charge / discharge process of the all-solid-state secondary battery (10), and improves the film strength of the inert member (40) by providing a bonding force between the support layer and other layers. The support layer provides support to the inert member (40), prevents unevenness of pressure applied to the solid electrolyte layer (30) during the pressurization process or the charge / discharge process, and prevents deformation of the all-solid-state secondary battery (1) being manufactured.

[0197] Referring to FIG. 14, the all-solid-state secondary battery (1) includes a positive electrode (10), a negative electrode (20), and a solid electrolyte layer (30, 30a, 30b) disposed therebetween, and the positive electrode layer (10) includes a positive electrode current collector (11) and a first positive electrode active material layer (12a) and a second positive electrode active material layer (12b) disposed on both sides of the positive electrode current collector (11), respectively, and the solid electrolyte layer (30) includes a first solid electrolyte layer (30a) in contact with the first positive electrode active material layer (12a) and a second solid electrolyte layer (30b) in contact with the second positive electrode active material layer (12b), and the negative electrode layer (20) includes a first negative electrode layer (20a) in contact with the first solid electrolyte layer (30a) and a second negative electrode layer (20b) in contact with the second solid electrolyte layer (30b), respectively. An inert member (40) is arranged to surround the side surface of the positive electrode layer (10) between the first solid electrolyte layer (30a) and the second solid electrolyte layer (30b) which face each other. The inert member (40) includes, for example, a first inert member (50a) which contacts the first solid electrolyte layer (30a) and a second inert member (40b) which contacts the second solid electrolyte layer (30b). Therefore, the all-solid-state secondary battery (1) has a bi-cell structure. Since the all-solid-state secondary battery (1) has such a bi-cell structure, the solid electrolyte layer (30) and the negative electrode layer (20) are arranged symmetrically to face each other with the positive electrode layer (10) as the center, so that structural deformation due to pressure applied during the manufacture of the all-solid-state secondary battery (1) is more effectively suppressed. Accordingly, cracking of the solid electrolyte layer (30) is suppressed during the manufacturing process and / or the charging / discharging process of the all-solid-state secondary battery (1), thereby preventing short circuit of the all-solid-state secondary battery (1), and consequently further improving the cycle characteristics of the all-solid-state secondary battery (1). In addition, since only one positive electrode collector (11) is used for a plurality of positive electrode active material layers (12a, 12b), the energy density of the all-solid-state secondary battery (1) is increased.

[0198] Referring to FIGS. 12 to 14, the inert member (40) is, for example, a flame-retardant inert member. By providing flame retardancy, the flame-retardant inert member can prevent thermal runaway and ignition of the all-solid-state secondary battery (1). Consequently, the safety of the all-solid-state secondary battery (1) is further improved. By being configured to absorb residual moisture within the all-solid-state secondary battery (1), the flame-retardant inert member prevents deterioration of the all-solid-state secondary battery (1), thereby improving the lifespan characteristics of the all-solid-state secondary battery (1).

[0199] The flame-retardant inert member includes, for example, a matrix and a filler. The matrix includes, for example, a substrate and a reinforcing material. The matrix includes, for example, a fibrous substrate and a fibrous reinforcing material. Since the matrix includes the substrate, the matrix can have elasticity. Therefore, the matrix can effectively accommodate a change in volume during charging and discharging of the all-solid-state secondary battery (1) and can be arranged at various positions. The substrate included in the matrix includes, for example, a first fibrous material. Since the substrate includes the first fibrous material, the volume change of the positive electrode layer (30) occurring during the charging and discharging process of the all-solid-state secondary battery (1) can be effectively accommodated and deformation of the first inert member (40) caused by the change in volume of the positive electrode layer (30) can be effectively suppressed. The first fibrous material is, for example, a material having an aspect ratio of 5 or more, 20 or more, or 50 or more. The first fibrous material is, for example, a material having an aspect ratio of 5 to 1000, 20 to 1000, or 50 to 1000. The first fibrous material is, for example, an insulating material. Since the first fibrous material is an insulating material, a short circuit between the positive electrode layer (30) and the negative electrode layer (20) caused by lithium dendrites, etc., generated during the charge and discharge process of the all-solid-state secondary battery (1) can be effectively prevented. The first fibrous material includes, for example, at least one selected from pulp fibers, insulating polymer fibers, and ion-conductive polymer fibers. The strength of the matrix is ​​improved by the inclusion of a reinforcing material in the matrix. Therefore, the matrix can prevent excessive volume change during charge and discharge of the all-solid-state secondary battery (1) and deformation of the all-solid-state secondary battery. The reinforcing material included in the matrix includes, for example, a second fibrous material. Since the reinforcing material includes the second fibrous material, the strength of the matrix can be increased more uniformly. The second fibrous material is, for example, a material having an aspect ratio of 3 or more, 5 or more, or 10 or more.The first fibrous material is, for example, a material having an aspect ratio of 3 to 100, 5 to 100, or 10 to 100. The second fibrous material is, for example, a flame-retardant material. Since the second fibrous material is a flame-retardant material, ignition due to thermal runaway occurring during the charge / discharge process of the all-solid-state secondary battery (1) or due to external impact can be effectively suppressed. The second fibrous material is, for example, glass fiber, metal oxide fiber, ceramic fiber, etc.

[0200] The flame-retardant inert member includes a filler in addition to a matrix. The filler may be disposed within the matrix, on the surface of the matrix, or on both the interior and the surface. The filler is, for example, an inorganic material. The filler included in the flame-retardant inert member is, for example, a moisture getter, a flame retardant, or a lithium immobilizer. The moisture getter removes moisture remaining in the all-solid-state secondary battery (1) by adsorbing moisture, for example, at a temperature below 100°C, thereby preventing deterioration of the all-solid-state secondary battery (1). In addition, when the temperature of the all-solid-state secondary battery (1) increases to 150°C or higher due to thermal runaway occurring during the charge / discharge process of the all-solid-state secondary battery (1) or an external impact, the moisture getter releases the adsorbed moisture, thereby effectively suppressing ignition of the all-solid-state secondary battery (1). The moisture getter is, for example, a metal hydroxide having moisture adsorption properties. The metal hydroxide included in the filler is, for example, Mg(OH)2, Fe(OH)3, Sb(OH)3, Sn(OH)4, TI(OH)3, Zr(OH)4, Al(OH)3, or a combination thereof. The flame retardant includes, for example, at least one selected from zinc borate, calcium molybdate zinc complex, MoO3, (NH4)2Mo2O7, Sb2O3, and Sb3O5. The lithium fixing agent may be, for example, a compound that reacts with liquid lithium to fixate lithium at a lithium melting temperature of 180°C or higher. The lithium fixing agent may react with liquid lithium to change lithium into another insoluble compound, for example. The lithium fixing agent is, for example, a metal oxide that is reactive with liquid lithium. The metal oxide included in the filler is, for example, TiO2, ZrO2, HfO2, ThO2, or a combination thereof. Metal oxides react with liquid lithium, for example, to produce Li2O and the metal.For example, the reaction formula is 4Li + MO2-> M + 2Li2O. Liquid lithium is fixed by reacting with a metal oxide to produce lithium oxide. Leakage of molten liquid lithium to the cathode at high temperatures can be suppressed. Therefore, the safety of all-solid-state secondary batteries can be improved.

[0201] The content of the filler included in the flame-retardant inert member is, for example, 1 to 80 parts by weight, 5 to 80 parts by weight, 10 to 80 parts by weight, 20 to 80 parts by weight, 30 to 80 parts by weight, 40 to 80 parts by weight, 50 to 80 parts by weight, 60 to 80 parts by weight, or 65 to 80 parts by weight, based on 100 parts by weight of the flame-retardant inert member (4).

[0202] The flame-retardant inert member may further comprise, for example, a binder. The binder may comprise, for example, a curable polymer or a non-curable polymer. A curable polymer is a polymer that cures by heat and / or pressure. A curable polymer is, for example, a solid at room temperature. The flame-retardant inert member may comprise, for example, a thermo-pressure curable film and / or a cured product thereof. An example of a thermo-pressure curable polymer is TSA-66 from Toray.

[0203] The flame-retardant inert member may additionally include other materials in addition to the above-described substrate, reinforcing material, filler, and binder. The flame-retardant inert member may further include one or more selected from among paper, an insulating polymer, an ion-conducting polymer, an insulating inorganic material, an oxide-based solid electrolyte, and a sulfide-based solid electrolyte. The insulating polymer may be, for example, an olefin-based polymer such as polypropylene (PP) or polyethylene (PE).

[0204] The density of the substrate or reinforcing material included in the flame-retardant inert material may be, for example, 10% to 300%, 10% to 150%, 10% to 140%, 10% to 130%, or 10% to 120% of the density of the positive electrode active material included in the lithium host layer (22).

[0205] The inert member (40) is a member that does not contain an electrochemically active material, for example, an electrode active material. The electrode active material is a material that absorbs / releases lithium. The inert member (40) is a member made of a material other than the electrode active material and used in the relevant technical field.

[0206]

[0207] [Solid electrolyte layer]

[0208] [Solid electrolyte layer: solid electrolyte]

[0209] Referring to FIGS. 6 to 14, the solid electrolyte layer (30) includes a solid electrolyte disposed between the positive electrode layer (10) and the negative electrode layer (20).

[0210] Referring to FIGS. 6 and 8, the solid electrolyte layer (30) may include, for example, a first two-dimensional sulfide-based solid electrolyte (100) arranged along one direction. By aligning the first two-dimensional sulfide-based solid electrolyte (100) along one direction, the density of the solid electrolyte layer (30) may be further improved. As a result, the energy density of the lithium battery may be further improved.

[0211] The direction in which the first two-dimensional sulfide-based solid electrolyte (100) is aligned may be, for example, a direction distinct from the thickness direction (y direction) of the solid electrolyte layer (30). The angle formed by the direction in which the first two-dimensional sulfide-based solid electrolyte (100) is aligned and the thickness direction of the solid electrolyte layer (30) may be, for example, 10 to 170 degrees, 20 to 160 degrees, 30 to 150 degrees, 14 to 135 degrees, 60 to 120 degrees, or 75 to 105 degrees.

[0212] The first two-dimensional sulfide-based solid electrolyte (100) may be aligned, for example, in a direction substantially orthogonal to the thickness direction of the solid electrolyte layer (z direction or x direction). That is, the first two-dimensional sulfide-based solid electrolyte (100) may be aligned such that the first surface (S1) and / or the second surface (S2) of the first two-dimensional sulfide-based solid electrolyte (100) are arranged in a direction parallel to the surface of the solid electrolyte layer (30).

[0213] By including a first two-dimensional sulfide-based solid electrolyte aligned along a direction distinct from the thickness direction of the solid electrolyte layer (30), the growth of lithium dendrites in the thickness direction of the solid electrolyte layer (30) can be suppressed and short circuits, etc. can be suppressed. As a result, deterioration of the all-solid-state secondary battery can be suppressed and the life characteristics can be improved.

[0214] The direction in which the first two-dimensional sulfide-based solid electrolyte (100) is laminated may be, for example, a direction similar to the thickness direction of the solid electrolyte layer (30). The angle formed by the direction in which the first two-dimensional sulfide-based solid electrolyte (100) is laminated and the thickness direction of the solid electrolyte layer (30) may be, for example, -30 to 30 degrees or -20 to 20 degrees. That is, the first two-dimensional sulfide-based solid electrolyte (100) may be laminated in the thickness direction of the solid electrolyte layer (30) such that the first surface (S1) and / or the second surface (S2) of the first two-dimensional sulfide-based solid electrolyte (100) are arranged in a direction parallel to the surface of the solid electrolyte layer (30).

[0215] The first two-dimensional sulfide-based solid electrolyte (100) may be laminated, for example, in the thickness direction of the solid electrolyte layer (30). The solid electrolyte layer (30) may include a first two-dimensional sulfide-based solid electrolyte laminate (200). The solid electrolyte layer (30) may include a plurality of first two-dimensional sulfide-based solid electrolyte laminates (200). The number of first two-dimensional sulfide-based solid electrolytes (100) included in one first two-dimensional sulfide-based solid electrolyte laminate (200) may be 2 or more, 5 or more, 10 or more, 50 or more, 100 or more, or 200 or more. The number of first two-dimensional sulfide-based solid electrolytes (100) included in one first two-dimensional sulfide-based solid electrolyte laminate (200) may be 2 to 1000, 5 to 1000, 10 to 1000, 50 to 1000, 100 to 1000, or 200 to 1000. Since the solid electrolyte layer (30) includes the first two-dimensional sulfide-based solid electrolyte (100) laminated along a direction similar to the thickness direction of the solid electrolyte layer (30), the growth of lithium dendrites in the thickness direction of the solid electrolyte layer (30) can be suppressed and short circuits, etc. can be suppressed. As a result, deterioration of the all-solid-state secondary battery can be suppressed and the life characteristics can be improved.

[0216] The content of the first two-dimensional sulfide-based solid electrolyte (100) may be, for example, 50 wt% or more, 60 wt% or more, 70 wt% or more, 80 wt% or more, 90 wt% or more, or 95 wt% or more of the total weight of the solid electrolyte layer (30). The content of the first two-dimensional sulfide-based solid electrolyte (100) may be, for example, 50 to 100 wt%, 60 to 100 wt%, 70 to 100 wt%, 80 to 100 wt%, 90 to 99.99 wt%, or 95 to 99 wt% of the total weight of the solid electrolyte layer (30). Since the solid electrolyte layer (30) includes such a high content of the first two-dimensional sulfide-based solid electrolyte (100), the possibility of generating pinholes (P) on the surface of the solid electrolyte layer (30) during the manufacture of the solid electrolyte layer (30) can be further reduced. Accordingly, the growth of lithium dendrites originating from the pinholes can be more effectively suppressed during charging and discharging of the all-solid-state secondary battery. As a result, the life characteristics of the all-solid-state secondary battery can be further improved.

[0217] In contrast, referring to FIGS. 7 and 9, in a solid electrolyte layer (30) including an amorphous sulfide-based solid electrolyte (100A) having an aspect ratio of less than 2, lithium dendrites can easily grow in the thickness direction of the solid electrolyte layer (30) because grain boundaries between particles of the amorphous sulfide-based solid electrolyte (100A) are connected in the thickness direction of the solid electrolyte layer (30). In addition, pinholes (P, pin-holes) are easily formed between particles of the amorphous sulfide-based solid electrolyte (100A) on the surface of the solid electrolyte layer (30), so that lithium dendrites can grow more easily through these pinholes. As a result, the possibility of a short circuit of a lithium battery including such a solid electrolyte layer (30) increases and the cycle characteristics deteriorate.

[0218] The first two-dimensional sulfide-based solid electrolyte (100) may be selected from among the sulfide-based solid electrolytes included in the cathode active material layer (12). Alternatively, the solid electrolyte layer (30) may include an oxide-based solid electrolyte, a polymer solid electrolyte, or a combination thereof.

[0219] The oxide-based solid electrolyte can be selected from among the oxide-based solid electrolytes used in the positive electrode active material layer (12).

[0220] The polymer solid electrolyte may include, for example, a dry polymer electrolyte, a gel polymer electrolyte, or a combination thereof.

[0221] A dry polymer electrolyte is an electrolyte that is a mixture of, for example, a lithium salt and a polymer. A dry polymer electrolyte is, for example, a polymer electrolyte that does not include a liquid electrolyte. The polymer included in the dry polymer electrolyte can be, for example, polyethylene oxide (PEO), polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyethylene oxide (PEO), poly(styrene-b-ethylene oxide) block copolymer (PS-PEO), poly(styrene-butadiene), poly(styrene-isoprene-styrene), poly(styrene-b-divinylbenzene) block copolymer, poly(styrene-ethylene oxide-styrene) block copolymer, or a combination thereof. The lithium salt can be any one that can be used as a lithium salt in the art. For example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2)(x and y are 1 to 20), LiCl, LiI or mixtures thereof.

[0222] A gel polymer electrolyte is an electrolyte that contains a liquid electrolyte and a polymer. The liquid electrolyte is, for example, a mixture of a lithium salt and an organic solvent. The polymer contained in the gel polymer electrolyte can be selected from the polymers contained in the dry polymer electrolyte. The lithium salt can be selected from the lithium salts used in the dry polymer electrolyte.

[0223] The solid electrolyte layer (30) may be impermeable to lithium polysulfide. Accordingly, side reactions between lithium polysulfide generated during charging and discharging of the sulfide-based positive electrode active material and the negative electrode layer can be prevented. Accordingly, the cycle characteristics of the all-solid-state secondary battery (1) including the solid electrolyte layer (30) can be improved.

[0224] [Solid electrolyte layer: binder]

[0225] The solid electrolyte layer (30) may include, for example, a binder. The binder included in the solid electrolyte layer (30) is not limited to, but may include, for example, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, etc., and any binder used in the relevant technical field may be used. The binder of the solid electrolyte layer (30) may be the same as or different from the binder included in the positive electrode active material layer (12) and the negative electrode active material layer (22). The binder may be omitted.

[0226] The binder content included in the solid electrolyte layer (30) is 0.1 to 10 wt%, 0.1 to 5 wt%, 0.1 to 3 wt%, 0.1 to 1 wt%, 0 to 0.5 wt%, or 0 to 0.1 wt% with respect to the total weight of the solid electrolyte layer (30).

[0227]

[0228] [Cathode layer]

[0229] [Cathode layer: Cathode active material]

[0230] Referring to FIGS. 10 to 14, the negative electrode layer (20) includes a first negative electrode active material layer (22). The first negative electrode active material layer (22) includes, for example, a negative electrode active material and a binder.

[0231] The negative electrode active material included in the first negative electrode active material layer (22) is, for example, a negative electrode material that can form an alloy or compound with lithium.

[0232] The negative electrode active material included in the first negative electrode active material layer (22) has, for example, a particle form. The average particle diameter of the negative electrode active material having a particle form is, for example, 4 ㎛ or less, 3 ㎛ or less, 2 ㎛ or less, 1 ㎛ or less, 500 nm or less, 300 nm or less, or 100 nm or less. The average particle diameter of the negative electrode active material having a particle form is, for example, 10 nm to 4 ㎛, 10 nm to 3 ㎛, 10 nm to 2 ㎛, 10 nm to 1 ㎛, 10 nm to 500 nm, 10 nm to 300 nm, or 10 nm to 100 nm. When the negative electrode active material has an average particle diameter in this range, reversible absorption and / or desorption of lithium can be facilitated during charge and discharge. The average particle size of the negative electrode active material is, for example, the median diameter (D50) measured using a laser particle size distribution meter.

[0233] The negative electrode active material included in the first negative electrode active material layer (22) includes, for example, at least one selected from among a carbon-based negative electrode active material and a metal or semi-metal negative electrode active material.

[0234] Carbon-based negative electrode materials include, for example, amorphous carbon, crystalline carbon, porous carbon, or a combination thereof.

[0235] The carbon-based negative electrode material is, in particular, amorphous carbon. Amorphous carbon includes, but is not limited to, carbon black (CB), acetylene black (AB), furnace black (FB), ketjen black (KB), and graphene, and any material classified as amorphous carbon in the relevant technical field is acceptable. Amorphous carbon is carbon that has no crystallinity or very low crystallinity, and is distinguished from crystalline carbon or graphite-based carbon.

[0236] The carbon-based negative electrode active material may be, for example, porous carbon. The porous carbon has a pore volume of, for example, 0.1 cc / g to 10.0 cc / g, 0.5 cc / g to 5 cc / g, or 0.1 cc / g to 1 cc / g. The porous carbon has an average pore diameter of, for example, 1 nm to 50 nm, 1 nm to 30 nm, or 1 nm to 10 nm. The porous carbon has a BET surface area of, for example, 100 m 2 / g to 3000 m 2 / g is.

[0237] The metal or metalloid negative electrode active material includes, but is not limited to, one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn), and any metal or metalloid negative electrode active material that forms an alloy or compound with lithium in the relevant technical field may be used. For example, nickel (Ni) does not form an alloy with lithium and therefore is not a metal negative electrode active material.

[0238] The first negative electrode active material layer (22) includes a type of negative electrode active material among these negative electrode active materials, or includes a mixture of a plurality of different negative electrode active materials. For example, the first negative electrode active material layer (22) includes only amorphous carbon, or includes at least one selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). Alternatively, the first negative electrode active material layer (22) includes a mixture of amorphous carbon and at least one selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The mixing ratio of the mixture of amorphous carbon and gold, etc., is a weight ratio, for example, 99:1 to 1:99, 10:1 to 1:2, 5:1 to 1:1, or 4:1 to 2:1, but is not necessarily limited to this range and is selected according to the required characteristics of the all-solid-state secondary battery (1). When the negative electrode active material has this composition, the cycle characteristics of the all-solid-state secondary battery (1) are further improved.

[0239] The negative electrode active material included in the first negative electrode active material layer (22) includes, for example, a mixture of first particles made of amorphous carbon and second particles made of a metal or a metalloid. The metal or metalloid includes, for example, gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). Alternatively, the metalloid is a semiconductor. The content of the second particles is 1 to 99 wt%, 1 to 60 wt%, 8 to 60 wt%, 10 to 50 wt%, 15 to 40 wt%, or 20 to 30 wt% based on the total weight of the mixture. When the second particles have a content in this range, the cycle characteristics of, for example, an all-solid-state secondary battery (1) are further improved.

[0240] Alternatively, the first negative electrode active material layer (22) includes a composite negative electrode active material. The composite negative electrode active material may include, for example, a carbon-based support and a metal-based negative electrode active material supported on the carbon-based support. Since the composite negative electrode active material has such a structure, the metal-based negative electrode active material can be prevented from being localized within the first negative electrode active material layer and a uniform distribution can be achieved. As a result, the cycle characteristics of the all-solid-state secondary battery (1) including the first negative electrode active material layer (22) are further improved.

[0241] The metal-based negative electrode active material supported on the carbon-based support includes, for example, a metal, a metal oxide, a composite of a metal and a metal oxide, or a combination thereof. The metal includes, for example, gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The metal oxide includes, for example, gold (Au) oxide, platinum (Pt) oxide, palladium (Pd) oxide, silicon (Si) oxide, silver (Ag) oxide, aluminum (Al) oxide, bismuth (Bi) oxide, tin (Sn) oxide, and zinc (Zn) oxide. The metal oxide includes, for example, Au x O y (0 <x≤2, 0<y≤3), Pt x O y (0 <x≤1, 0<y≤2), Pd x O y (0 <x≤1, 0<y≤1), Si x O y (0 <x≤1, 0<y≤2), Ag x O y (0 <x≤2, 0<y≤1), Al x O y (0 <x≤2, 0<y≤3), Bi x O y (0 <x≤2, 0<y≤3), Sn x O y (0 <x≤1, 0<y≤2), Zn x O y(0 <x≤1, 0<y≤1), 또는 이들의 조합을 포함할 수 있다. 금속과 금속산화물의 복합체는 예를 들어 Au와 Au x O y (0 <x≤2, 0<y≤3)의 복합체, Pt와 Pt x O y (0 <x≤1, 0<y≤2)의 복합체, Pd와 Pd x O y (0 <x≤1, 0<y≤1)의 복합체, Si와 Si x O y (0 <x≤1, 0<y≤2)의 복합체, Ag 와 Ag x O y (0 <x≤2, 0<y≤1)의 복합체, Al과 Al x O y (0 <x≤2, 0<y≤3)의 복합체, Bi와 Bi x O y (0 <x≤2, 0<y≤3)의 복합체, Sn과 Sn x O y (0 <x≤1, 0<y≤2)의 복합체, Zn과 Zn x O y (0 <x≤1, 0<y≤1)의 복합체, 또는 이들의 조합을 포함할 수 있다.

[0242] The carbonaceous support is, for example, amorphous carbon. Amorphous carbon includes, but is not limited to, carbon black (CB), acetylene black (AB), furnace black (FB), ketjen black (KB), graphene, activated carbon, carbon nanofibers (CNF), carbon nanotubes (CNT), etc., and any material classified as amorphous carbon in the relevant technical field is possible. Amorphous carbon is carbon that has no crystallinity or very low crystallinity, and is distinguished from crystalline carbon or graphite carbon. Carbonaceous materials are, for example, carbonaceous negative electrode active materials.

[0243] The composite negative electrode active material may have, for example, a particle form. The particle size of the composite negative electrode active material having a particle form is, for example, 10 nm to 4 ㎛, 10 nm to 1 ㎛, 10 nm to 500 nm, 10 nm to 200 nm, or 10 nm to 100 nm. When the composite negative electrode active material has a particle size in this range, reversible absorption and / or desorption of lithium may be facilitated during charge and discharge. The metal-based negative electrode active material supported on the support may have, for example, a particle form. The particle size of the metal-based negative electrode active material may be, for example, 1 nm to 200 nm, 1 nm to 150 nm, 5 nm to 100 nm, or 10 nm to 50 nm. The carbon-based support may have, for example, a particle form. The particle size of the carbon-based support may be, for example, 10 nm to 2 ㎛, 10 nm to 1 ㎛, 10 nm to 500 nm, 10 nm to 200 nm, or 10 nm to 100 nm. By having a particle size in this range, the carbon-based support can be more uniformly arranged within the first negative electrode active material layer. The carbon-based support may be, for example, nanoparticles having a particle size of 500 nm or less. The particle sizes of the composite negative electrode active material, the particle sizes of the metal-based negative electrode active material, and the particle sizes of the carbon-based support are, for example, average particle sizes. The average particle size is, for example, the median diameter (D50) measured using a laser particle size distribution analyzer. Alternatively, the average particle size may be determined automatically using software, for example, from an electron microscope image, or manually by a manual method.

[0244] [Cathode layer: binder]

[0245] The binder included in the first negative electrode active material layer (22) is, for example, styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, vinylidene fluoride / hexafluoropropylene copolymer, polyacrylonitrile, polymethyl methacrylate, etc., but is not necessarily limited thereto and any binder used in the relevant technical field may be used. The binder may be composed of a single binder or a plurality of different binders.

[0246] Since the first negative electrode active material layer (22) includes a binder, the first negative electrode active material layer (22) is stabilized on the negative electrode current collector (21). In addition, cracking of the first negative electrode active material layer (22) is suppressed despite changes in the volume and / or relative position of the first negative electrode active material layer (22) during the charge and discharge process. For example, if the first negative electrode active material layer (22) does not include a binder, the first negative electrode active material layer (22) can be easily separated from the negative electrode current collector (21). As the first negative electrode active material layer (22) is detached from the negative electrode current collector (21), the possibility of a short circuit occurring increases at the exposed portion of the negative electrode current collector (21) due to the negative electrode current collector (21) coming into contact with the solid electrolyte layer (30). The first negative electrode active material layer (22) is manufactured by, for example, applying a slurry in which the material constituting the first negative electrode active material layer (22) is dispersed onto the negative electrode current collector (21) and drying the slurry. By including a binder in the first negative electrode active material layer (22), stable dispersion of the negative electrode active material in the slurry is possible. For example, when applying the slurry onto the negative electrode current collector (21) by screen printing, it is possible to suppress clogging of the screen (for example, clogging by aggregates of the negative electrode active material).

[0247] [Cathode layer: Other additives]

[0248] The first negative electrode active material layer (22) may further include additives used in a conventional all-solid-state secondary battery (1), such as fillers, coating agents, dispersants, and ion conductive aids.

[0249] [Cathode layer: solid electrolyte]

[0250] The first negative electrode active material layer (22) may further include a solid electrolyte. The solid electrolyte may be, for example, a material selected from among the solid electrolytes included in the solid electrolyte layer (30). The solid electrolyte included in the first negative electrode active material layer (22) may act as a reaction site where lithium metal formation begins within the first negative electrode active material layer (22), as a space where the formed lithium metal is stored, or as a path for transferring lithium ions. The solid electrolyte may be omitted.

[0251] In the first negative electrode active material layer (22), the content of the solid electrolyte may be high, for example, in an area adjacent to the solid electrolyte layer (30), and low, for example, in an area adjacent to the negative electrode current collector (21). In the first negative electrode active material layer (22), the solid electrolyte may have a concentration gradient in which the concentration decreases, for example, from an area adjacent to the solid electrolyte layer (30) to an area adjacent to the negative electrode current collector (21).

[0252] [Cathode layer: first cathode active material layer]

[0253] The initial charge capacity (B) of the first negative electrode active material layer is less than 50%, 45% or less, 40% or less, 30% or less, 20% or less, or 10% or less of the initial charge capacity (A) of the positive electrode active material layer. For example, the ratio (B / A) of the initial charge capacity (B) of the first negative electrode active material layer (22) and the initial charge capacity (A) of the positive electrode active material layer is 0.005 to 0.45. The initial charge capacity of the positive electrode active material layer (12) is a first open circuit voltage (1 st Li / Li from open circuit voltage) +The initial charge capacity of the first negative electrode active material layer (22) is determined at the maximum charging voltage. The initial charge capacity of the first negative electrode active material layer (22) is determined at the second open circuit voltage (2 nd Li / Li from open circuit voltage) + It is determined at 0.01 V.

[0254] The maximum charge voltage is determined by the type of cathode active material. The maximum charge voltage can be, for example, 1.5 V, 2.0 V, 2.5 V, 2.8 V, 3.0 V, 3.5 V, 4.0 V, 4.2 V, or 4.3 V. For example, the maximum charge voltage of Li2S or Li2S composite is Li / Li + can be 2.5 V for Li2S or Li2S complex. For example, the maximum charging voltage of Li / Li + It can be 3.0 V for. The ratio (B / A) of the initial charge capacity (B) of the first negative electrode active material layer (22) and the initial charge capacity (A) of the positive electrode active material layer is, for example, 0.001 to less than 0.5, 0.01 to 0.45, 0.01 to 0.4, 0.01 to 0.3, 0.01 to 0.2, or 0.05 to 0.1.

[0255] The initial charge capacity (mAh) of the positive electrode active material layer (12) is obtained by multiplying the charge capacity density (charge specific capacity) (mAh / g) of the positive electrode active material by the mass (g) of the positive electrode active material in the positive electrode active material layer (12). When multiple types of positive electrode active materials are used, the charge capacity density × mass value is calculated for each positive electrode active material, and the sum of these values ​​is the initial charge capacity of the positive electrode active material layer (12). The initial charge capacity of the first negative electrode active material layer (22) is also calculated in the same way. The initial charge capacity of the first negative electrode active material layer (22) is obtained by multiplying the charge capacity density (mAh / g) of the negative electrode active material by the mass of the negative electrode active material in the first negative electrode active material layer (22). When multiple types of negative electrode active materials are used, the charge capacity density × mass value is calculated for each negative electrode active material, and the sum of these values ​​is the initial charge capacity of the first negative electrode active material layer (22). The charge capacity density of each of the positive electrode active material and the negative electrode active material can be measured using an all-solid-state half-cell using lithium metal as a counter electrode. The initial charge capacity of each of the positive electrode active material layer (12) and the first negative electrode active material layer (22) is measured at a constant current density, for example, 0.1 mA / cm 2 can be directly measured using an all-solid-state half-cell. For the positive electrode, the measurement is made from the first open circuit voltage (OCV) to the maximum charge voltage, e.g., 3.0 V (vs. Li / Li + ) can be performed for an operating voltage of up to 0.01 V for the cathode, for example, lithium metal, from the second open circuit voltage (OCV). For example, an all-solid-state half-cell having a cathode active material layer can measure a current of 0.1 mA / cm from the first open circuit voltage to 3.0 V. 2 The all-solid-state half-cell having the first negative active material layer is charged with a constant current of 0.1 mA / cm from the second open circuit voltage to 0.01 V. 2It can be charged with a constant current. The current density during constant current charging is, for example, 0.2 mA / cm 2 , or 0.5 mA / cm 2 The all-solid-state half-cell having the positive electrode active material layer can be charged from the first open circuit voltage to, for example, 2.5 V, 2.0 V, 3.5 V, or 4.0 V. The maximum charge voltage of the positive electrode active material layer can be determined by the maximum voltage of the battery that satisfies the safety conditions according to JISC8712:2015 of the Japanese Standards Association.

[0256] If the initial charge capacity of the first negative electrode active material layer (22) is too small, the thickness of the first negative electrode active material layer (22) becomes very thin, so that lithium dendrites formed between the first negative electrode active material layer (22) and the negative electrode current collector (21) during repeated charge / discharge processes collapse the first negative electrode active material layer (22), making it difficult to improve the cycle characteristics of the all-solid-state secondary battery (1). If the charge capacity of the first negative electrode active material layer (22) increases excessively, the energy density of the all-solid-state secondary battery (1) decreases and the internal resistance of the all-solid-state secondary battery (1) due to the first negative electrode active material layer (22) increases, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery (1).

[0257] The thickness of the first negative electrode active material layer (22) is, for example, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, or 5% or less of the thickness of the positive electrode active material layer (12). The thickness of the first negative electrode active material layer (22) is, for example, 1 to 50%, 1 to 40%, 1 to 30%, 1 to 20%, 1 to 10%, or 1 to 5% of the thickness of the positive electrode active material layer (12). The thickness of the first negative electrode active material layer (22) is, for example, 1 µm to 20 µm, 2 µm to 15 µm, or 3 µm to 10 µm. If the thickness of the first negative electrode active material layer (22) is too thin, lithium dendrites formed between the first negative electrode active material layer (22) and the negative electrode current collector (21) collapse the first negative electrode active material layer (22), making it difficult to improve the cycle characteristics of the all-solid-state secondary battery (1). If the thickness of the first negative electrode active material layer (22) increases excessively, the energy density of the all-solid-state secondary battery (1) decreases and the internal resistance of the all-solid-state secondary battery (1) due to the first negative electrode active material layer (22) increases, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery (1). If the thickness of the first negative electrode active material layer (22) decreases, for example, the initial charge capacity of the first negative electrode active material layer (22) also decreases.

[0258] [Cathode layer: second cathode active material layer]

[0259] Although not shown in the drawing, the all-solid-state secondary battery (1) further includes, after being charged, a second negative electrode active material layer disposed, for example, between the negative electrode current collector (21) and the first negative electrode active material layer (22). The second negative electrode active material layer is a metal layer containing lithium or a lithium alloy. The metal layer contains lithium or a lithium alloy. Therefore, since the second negative electrode active material layer is a metal layer containing lithium, it functions as, for example, a lithium reservoir. The lithium alloy is, for example, a Li-Al alloy, a Li-Sn alloy, a Li-In alloy, a Li-Ag alloy, a Li-Au alloy, a Li-Zn alloy, a Li-Ge alloy, a Li-Si alloy, etc., but is not limited thereto, and any lithium alloy used in the art may be used. The second negative electrode active material layer may be made of one of these alloys or lithium, or may be made of several types of alloys. The second negative electrode active material layer is, for example, a plated layer. The second negative electrode active material layer is deposited between the first negative electrode active material layer (22) and the negative electrode current collector (21), for example, during the charging process of an all-solid-state secondary battery (1).

[0260] The thickness of the second negative electrode active material layer is not particularly limited, but is, for example, 1 ㎛ to 500 ㎛, 1 ㎛ to 200 ㎛, 1 ㎛ to 150 ㎛, 1 ㎛ to 100 ㎛, or 1 ㎛ to 50 ㎛. If the thickness of the second negative electrode active material layer is too thin, it is difficult for the second negative electrode active material layer to perform the role of a lithium reservoir. If the thickness of the second negative electrode active material layer is too thick, the mass and volume of the all-solid-state secondary battery (1) may increase, and the cycle characteristics of the all-solid-state secondary battery (1) may rather deteriorate.

[0261] Alternatively, in the all-solid-state secondary battery (1), the second negative electrode active material layer may be disposed between the negative electrode current collector (21) and the first negative electrode active material layer (22), for example, before assembling the all-solid-state secondary battery (1). When the second negative electrode active material layer (23) is disposed between the negative electrode current collector (21) and the first negative electrode active material layer (22) before assembling the all-solid-state secondary battery (1), the second negative electrode active material layer acts as a lithium reservoir because it is a metal layer containing lithium. For example, a lithium foil may be disposed between the negative electrode current collector (21) and the first negative electrode active material layer (22) before assembling the all-solid-state secondary battery (1).

[0262] When the second negative electrode active material layer is precipitated by charging after assembling the all-solid-state secondary battery (1), the energy density of the all-solid-state secondary battery (1) increases because the second negative electrode active material layer is not included when assembling the all-solid-state secondary battery (1). When charging the all-solid-state secondary battery (1), the charging is performed in excess of the charging capacity of the first negative electrode active material layer (22). That is, the first negative electrode active material layer (22) is overcharged. At the beginning of charging, lithium is absorbed into the first negative electrode active material layer (22). The negative electrode active material included in the first negative electrode active material layer (22) forms an alloy or compound with the lithium ions that have moved from the positive electrode layer (10). When charging exceeds the capacity of the first negative electrode active material layer (22), for example, lithium is deposited on the back surface of the first negative electrode active material layer (22), that is, between the negative electrode current collector (21) and the first negative electrode active material layer (22), and a metal layer corresponding to the second negative electrode active material layer is formed by the deposited lithium. The second negative electrode active material layer is a metal layer mainly composed of lithium (i.e., metallic lithium). This result is obtained, for example, by the negative electrode active material included in the first negative electrode active material layer (22) including a material that forms an alloy or compound with lithium. During discharge, lithium in the first negative electrode active material layer (22) and the second negative electrode active material layer, that is, the metal layer, is ionized and moves toward the positive electrode layer (10). Therefore, it is possible to use lithium as the negative electrode active material in an all-solid-state secondary battery (1). In addition, since the first negative electrode active material layer (22) covers the second negative electrode active material layer, it functions as a protective layer for the second negative electrode active material layer, i.e., the metal layer, and at the same time, it suppresses the precipitation and growth of lithium dendrites. Accordingly, it suppresses short circuits and capacity reduction of the all-solid-state secondary battery (1), and consequently improves the cycle characteristics of the all-solid-state secondary battery (1).In addition, when the second negative electrode active material layer is disposed by charging after assembling the all-solid-state secondary battery (1), the negative electrode layer (20), i.e., the negative electrode current collector (21) and the first negative electrode active material layer (22) and the region between them are Li-free regions that do not contain lithium (Li) in the initial state or the state after complete discharge of the all-solid-state secondary battery (1).

[0263] [Cathode layer: negative current collector]

[0264] The negative electrode current collector (21) is composed of, for example, a material that does not react with lithium, i.e., does not form an alloy or a compound. The material constituting the negative electrode current collector (21) is, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), and nickel (Ni), but is not necessarily limited thereto, and any material that can be used as an electrode current collector in the relevant technical field can be used. The negative electrode current collector (21) may be composed of one type of the above-described metal, or may be composed of an alloy or a coating material of two or more types of metals. The negative electrode current collector (21) is, for example, in the form of a plate or foil.

[0265] The all-solid-state secondary battery (1) may further include, for example, a thin film containing an element capable of forming an alloy with lithium on one surface of the negative electrode current collector (21), although not shown in the drawing. The thin film is disposed between the negative electrode current collector (21) and the first negative electrode active material layer (22). The thin film contains, for example, an element capable of forming an alloy with lithium. The element capable of forming an alloy with lithium includes, but is not limited to, gold, silver, zinc, tin, indium, silicon, aluminum, bismuth, etc., and any element capable of forming an alloy with lithium in the art may be used. The thin film may be composed of one of these metals or an alloy of several types of metals. By placing the thin film on one surface of the negative electrode current collector (21), for example, the deposition shape of the second negative electrode active material layer deposited between the thin film (24) and the first negative electrode active material layer (22) becomes flatter, and the cycle characteristics of the all-solid-state secondary battery (1) can be further improved.

[0266] The thickness of the thin film is, for example, 1 nm to 800 nm, 10 nm to 700 nm, 50 nm to 600 nm, or 100 nm to 500 nm. If the thickness of the thin film is less than 1 nm, it may be difficult for the function of the thin film to be exerted. If the thickness of the thin film is excessively thick, the thin film itself may absorb lithium, which may reduce the amount of lithium precipitation from the negative electrode, thereby lowering the energy density of the all-solid-state battery and deteriorating the cycle characteristics of the all-solid-state secondary battery (1). The thin film may be disposed on the negative electrode current collector (21) by, for example, a vacuum deposition method, a sputtering method, a plating method, or the like, but is not necessarily limited to these methods, and any method capable of forming a thin film in the relevant technical field may be used.

[0267] Although not shown in the drawing, the negative electrode current collector (21) may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. The polymer may be an insulating polymer. Since the base film includes an insulating thermoplastic polymer, when a short circuit occurs, the base film may soften or liquefy, thereby blocking battery operation and suppressing a rapid increase in current. The metal layer may include, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), or an alloy thereof. The negative electrode current collector (21) may additionally include a metal piece and / or a lead tab. For more specific details regarding the base film, metal layer, metal chip, and lead tab of the negative electrode collector (21), refer to the positive electrode collector (11) described above. By having this structure, the negative electrode collector (21) can reduce the weight of the negative electrode, and consequently, improve the energy density of the negative electrode and lithium battery.

[0268]

[0269] The present invention is explained in more detail through the following examples and comparative examples. However, the examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention.

[0270] (two-dimensional sulfide solid electrolyte)

[0271] Manufacturing Example 1: First two-dimensional sulfide-based solid electrolyte

[0272] A reduced graphene oxide (rGO)-Li6PS5Cl composite was prepared as the first two-dimensional solid electrolyte. The rGO-Li6PS5Cl composite was prepared according to the method disclosed in Materials Today Energy 23 (2022) 100913, except that the weight ratio of rGO to Li6PS5Cl was changed to 1:60. The rGO-Li6PS5Cl composite is a Li6PS5Cl shell, which is an argyrodite-type crystal, coated on an rGO core. The rGO-Li6PS5Cl composite has a flake shape with a thickness of approximately 1 μm, a length of approximately 3 μm, and an aspect ratio of 3. The plane view of the rGO-Li6PS5Cl composite is a polygonal shape. The thickness and length of the rGO-Li6PS5Cl composite are average values ​​calculated from multiple composite particles read from scanning electron microscope images.

[0273]

[0274] (all-solid-state secondary battery)

[0275] Example 1: Mono-cell all-solid-state secondary battery, sulfide-based cathode active material (Li2S-C-LiI composite), flake solid electrolyte: particle-like solid electrolyte = 10:40 weight ratio, first two-dimensional solid electrolyte

[0276] (Cathode layer manufacturing)

[0277] A 10 ㎛ thick SUS foil was prepared as a negative electrode current collector. In addition, carbon black (CB) particles with a primary particle diameter of approximately 30 nm and silver (Ag) particles with an average particle diameter of approximately 60 nm were prepared as negative electrode active materials.

[0278] A mixed powder of 4 g of carbon black (CB) and silver (Ag) particles in a weight ratio of 3:1 was placed in a container, and 4 g of an NMP solution containing 7 wt% of PVDF binder (Kureha #9300) was added thereto to prepare a mixed solution. NMP (N-methyl-2-pyrrolidone) was added little by little to the prepared mixed solution and the mixed solution was stirred to prepare a slurry. The prepared slurry was applied to a SUS sheet using a bar coater and dried in air at 80°C for 10 minutes to prepare a laminate. The prepared laminate was vacuum-dried at 40°C for 10 hours. The dried laminate was cold roll pressed to flatten the surface of the first negative electrode active material layer of the laminate, thereby producing a negative electrode layer. The thickness of the first negative electrode active material layer was approximately 15 μm. The areas of the first negative electrode active material layer and the negative electrode current collector were the same. The initial charge capacity of the cathode layer (i.e., the first cathode active material layer) was measured using the half-cell described above.

[0279] (Anode layer manufacturing)

[0280] A Li2S-C-LiI composite was prepared as a cathode active material. The Li2S-C-LiI composite was prepared according to the method disclosed in Nano Lett. 2016, 16, 7, 4521-4527, except that Li6PS5Cl was changed to LiI. The rGO (reduced graphene oxide)-Li6PS5Cl composite prepared in Preparation Example 1 was prepared as the first two-dimensional solid electrolyte. Li6PS5Cl (D50 = 3.0 μm, crystalline), which is an argyrodite-type crystal, was prepared as an irregular-shaped particulate solid electrolyte. Ketjen black was prepared as a conductive agent. The aspect ratio of the irregular particulate solid electrolyte was less than 2.

[0281] These materials were mixed in a weight ratio of 40:10:40:10 (positive electrode active material): first two-dimensional solid electrolyte: amorphous particulate solid electrolyte: conductive agent) to prepare a positive electrode mixture. The positive electrode mixture was obtained by dry mixing using a ball mill. The positive electrode mixture obtained by ball milling formed an ionic conductive and electronic conductive network.

[0282] The positive electrode mixture was placed on one side of a carbon-coated aluminum foil positive electrode collector and plate pressed at a pressure of 200 MPa for 10 minutes to manufacture a positive electrode layer. The thickness of the positive electrode layer was about 120 ㎛. The thickness of the positive electrode active material layer was about 100 ㎛, and the thickness of the carbon-coated aluminum foil was about 20 ㎛. The areas of the positive electrode active material layer and the positive electrode collector were the same. The initial charge capacity of the positive electrode layer (i.e., the positive electrode active material layer) was measured using the half-cell described above. The ratio (B / A) of the initial charge capacity (B) of the first negative electrode active material layer and the initial charge capacity (A) of the positive electrode active material layer was less than 0.5. The initial charge capacity of the positive electrode active material layer was measured at the first open circuit voltage (1 st 2.8 V vs. Li / Li from open circuit voltage) + was determined by the charge up to . The initial charge capacity of the first negative active material layer was determined by the second open circuit voltage (2 nd 0.01 V vs. Li / Li from open circuit voltage) + It was determined by the charging up to . In addition, in Examples 2 to 10 and 12, the ratio (B / A) was less than 0.5, respectively.

[0283]

[0284] (Manufacturing of solid electrolyte layer)

[0285] A mixture was prepared by adding 1.5 parts by weight of an acrylic binder to 98.5 parts by weight of the solid electrolyte, Li6PS5Cl, which is an argyrodite-type crystal (D50 = 3.0 ㎛, crystalline). Octyl acetate was added to the prepared mixture and stirred to prepare a slurry. The prepared slurry was applied using a bar coater onto a 15 (m) thick nonwoven fabric placed on a 75 (m) thick PET substrate, and dried in air at 80°C for 10 minutes to obtain a laminate. The obtained laminate was vacuum-dried at 80°C for 2 hours. A solid electrolyte layer was prepared by the above process.

[0286] (flame retardant inert material)

[0287] A flame-retardant inert member was manufactured by forming a slurry containing pulp fiber (cellulose fiber), glass fiber, aluminum hydroxide (Al(OH)3), an acrylic binder, and a solvent into a gasket shape and then removing the solvent.

[0288] The weight ratio of pulp fiber (cellulose fiber), glass fiber, aluminum hydroxide (Al(OH)3), and acrylic binder was 20:8:70:2. The thickness of the inert material was 120 ㎛.

[0289] Before placing the manufactured flame-retardant inert material on the solid electrolyte layer, moisture, etc. of the flame-retardant inert material was removed by vacuum heat treatment at 80°C for 5 hours.

[0290] (Manufacturing of all-solid-state secondary batteries)

[0291] Referring to Fig. 1, a solid electrolyte layer was placed on the cathode layer such that the first cathode active material layer was in contact with the solid electrolyte layer. A flame-retardant inert material was placed on the solid electrolyte layer by heat and pressure to prepare a cathode layer / solid electrolyte layer / inert material laminate.

[0292] An anode layer / solid electrolyte layer / anode layer electrode assembly was prepared by arranging the inert member on one side of the anode layer so as to face the cathode active material layer. The inert member was arranged to surround the side of the anode layer and contact the solid electrolyte layer. The inert member was used as a gasket. The anode layer was arranged on the center of the solid electrolyte layer, and the gasket was arranged to surround the anode layer and extend to the end of the solid electrolyte layer. The area of ​​the anode layer was approximately 90% of the area of ​​the solid electrolyte layer, and the gasket was arranged over the entire area of ​​the remaining 10% of the solid electrolyte layer where the anode layer was not arranged.

[0293] The prepared cathode layer / solid electrolyte layer / anode layer electrode assembly was plate pressed. This pressing process sintered the solid electrolyte layer, thereby improving battery characteristics. The thickness of the sintered solid electrolyte layer was approximately 45 μm. The sintered electrode assembly was placed in a pouch and sealed to prepare a sealed electrode assembly. Portions of the cathode current collector and anode current collector were protruded outside the sealed electrode assembly to be used as the cathode layer terminal and the anode layer terminal.

[0294] An electrode assembly was placed between two press plates (not shown) and the two press plates were fastened with screws to apply a constant pressure to both sides of the electrode assembly, thereby manufacturing an all-solid-state secondary battery.

[0295] Example 2: Mono-cell all-solid-state secondary battery, sulfide-based cathode active material (Li2S-C-LiI composite), flake solid electrolyte: particle-like solid electrolyte = 5:45 weight ratio (including the first two-dimensional solid electrolyte)

[0296] A solid-state secondary battery was manufactured in the same manner as in Example 1, except that the weight ratio of the flake solid electrolyte to the particle solid electrolyte was changed to 5:45.

[0297] Example 3: Mono-cell all-solid-state secondary battery, sulfide-based cathode active material (Li2S-C-LiI composite), flake solid electrolyte: particle-like solid electrolyte = 20:20 weight ratio (including the first two-dimensional solid electrolyte)

[0298] Flake solid electrolyte: An all-solid-state secondary battery was manufactured in the same manner as Example 1, except that the weight ratio of the particle-type solid electrolyte was changed to 20:20.

[0299] Example 4: Mono-cell all-solid-state secondary battery, sulfide-based cathode active material (Li2S-C-LiI composite), flake solid electrolyte: particle-like solid electrolyte = 30:20 weight ratio (including first two-dimensional solid electrolyte)

[0300] Flake solid electrolyte: An all-solid-state secondary battery was manufactured in the same manner as Example 1, except that the weight ratio of the particle-type solid electrolyte was changed to 30:20.

[0301] Example 5: Mono-cell all-solid-state secondary battery, sulfide-based cathode active material (Li2S-C-LiI composite), flake solid electrolyte: particle-like solid electrolyte = 40:10 weight ratio (including the first two-dimensional solid electrolyte)

[0302] Flake solid electrolyte: An all-solid-state secondary battery was manufactured in the same manner as Example 1, except that the weight ratio of the particle-type solid electrolyte was changed to 40:10.

[0303]

[0304] Example 6: Mono-cell all-solid-state secondary battery, sulfide-based cathode active material (Li2S-C-LiI-2D solid electrolyte composite), flake solid electrolyte: particle-like solid electrolyte = 10:40 weight ratio, first and second two-dimensional solid electrolytes

[0305] An all-solid-state secondary battery was manufactured in the same manner as in Example 1, except that a Li2S-C-LiI-2D solid electrolyte composite was used instead of a Li2S-C-LiI composite as the cathode active material.

[0306] The Li2S-C-LiI-2D solid electrolyte composite was prepared by the following method.

[0307] A Li2S-C-LiI complex was prepared in the same manner as in Example 1. A 4:1 weight ratio mixture of the Li2S-C-LiF complex and the rGO (reduced graphene oxide)-Li6PS5Cl complex prepared in Preparation Example 1 was mixed at low speed using a mixer, and then complexed again using a mixer at a rotation speed of about 100 to 2000 rpm for about 0.1 to 20 hours to prepare a Li2S-C-LiI-2D solid electrolyte complex.

[0308] Example 7: Mono-cell all-solid-state secondary battery, sulfide-based cathode active material (Li2S-C-LiI-2D solid electrolyte composite), flake solid electrolyte: particle-like solid electrolyte = 0:50 weight ratio, second two-dimensional solid electrolyte

[0309] An all-solid-state secondary battery was manufactured in the same manner as in Example 1, except that the Li2S-C-LiI-2D solid electrolyte composite used in Example 6 was used instead of the Li2S-CNF composite as the cathode active material, and the weight ratio of the flake solid electrolyte and the particulate solid electrolyte in the cathode mixture was changed to 0:50 and the plate solid electrolyte was not used.

[0310] Example 8: Mono-cell all-solid-state secondary battery, sulfide-based cathode active material (Li2S-C-LiI composite), flake solid electrolyte: particle-like solid electrolyte = 10:40 weight ratio, two-layer cathode active material layer (arranged on top of flake solid electrolyte)

[0311] A first positive electrode mixture was prepared using the same method as in Example 1.

[0312] A second positive electrode mixture was prepared in the same manner as Example 1, except that the weight ratio of the flake solid electrolyte and the particle solid electrolyte was changed to 0:50 and the flake solid electrolyte was not used.

[0313] An all-solid-state secondary battery was manufactured in the same manner as Example 1, except that the first positive electrode mixture (containing a flake solid electrolyte) and the second positive electrode mixture (without a flake solid electrolyte) were sequentially arranged on the positive electrode current collector to manufacture the positive electrode layer.

[0314] The positive electrode active material layer includes a first positive electrode active material layer derived from a first positive electrode mixture and a second positive electrode active material layer derived from a second positive electrode mixture, and their thicknesses were each 50 μm.

[0315] The first cathode active material layer adjacent to the cathode current collector contained a plate solid electrolyte, and the second cathode active material layer adjacent to the solid electrolyte layer did not contain a flake solid electrolyte.

[0316] Example 9: Mono-cell all-solid-state secondary battery, sulfide-based cathode active material (Li2S-C-LiI composite), flake solid electrolyte: particle-like solid electrolyte = 10:40 weight ratio, two-layer cathode active material layer (flake solid electrolyte placed at the bottom)

[0317] An all-solid-state secondary battery was manufactured in the same manner as in Example 8, except that the positions of the first and second positive electrode active material layers were reversed, the second positive electrode active material layer was disposed adjacent to the positive electrode current collector, and the first positive electrode active material layer was disposed adjacent to the solid electrolyte layer. The second positive electrode active material layer adjacent to the positive electrode current collector contained a flake solid electrolyte, and the first positive electrode active material layer adjacent to the solid electrolyte layer did not contain a flake solid electrolyte.

[0318] Example 10: Mono-cell all-solid-state secondary battery, oxide-based cathode active material (NCA), flake solid electrolyte: particle-type solid electrolyte = 10:40 weight ratio

[0319] (Anode layer manufacturing)

[0320] LiNi coated with Li2O-ZrO2 (LZO) as a cathode active material 0.8 Co 0.15 Mn 0.05 O2(NCM) was prepared. The LZO-coated cathode active material was prepared according to the method disclosed in Korean Patent Publication No. 10-2016-0064942. The rGO (reduced graphene oxide)-Li6PS5Cl composite prepared in Manufacturing Example 1 was prepared as the first two-dimensional solid electrolyte. Li6PS5Cl, an argyrodite-type crystal (D50 = 0.5 μm, crystalline), was prepared as an irregular-shaped particulate solid electrolyte. Polytetrafluoroethylene (PTFE) binder was prepared as a binder. Carbon nanofibers (CNF) were prepared as a conductive agent. These materials were mixed with xylene solvent in a weight ratio of positive electrode active material: first two-dimensional solid electrolyte: amorphous particle-like solid electrolyte: conductive agent: binder = 84: 2: 9.5: 3: 1.5, and the slurry was molded into a sheet shape, and then vacuum dried at 40°C for 8 hours to manufacture a positive electrode sheet. The manufactured positive electrode sheet was placed on the carbon layer of a positive electrode current collector made of aluminum foil coated with a carbon layer on one side, and 85 o The positive electrode layer was manufactured by heated roll pressing of C. The total thickness of the positive electrode layer was approximately 120 μm. The thickness of each positive electrode active material layer was approximately 95 μm, and the thickness of the carbon-coated aluminum foil was approximately 25 μm.

[0321] (All-solid-state secondary battery manufacturing)

[0322] An all-solid-state secondary battery was manufactured in the same manner as in Example 1, except that the above-described positive electrode layer was used.

[0323] Example 11: Mono-cell all-solid-state secondary battery, oxide-based cathode active material (NCA), flake solid electrolyte: particle-like solid electrolyte = 10:40 weight ratio, first two-dimensional solid electrolyte, solid electrolyte layer is first two-dimensional solid electrolyte laminate

[0324] (Anode layer manufacturing)

[0325] LiNi coated with Li2O-ZrO2 (LZO) as a cathode active material 0.8 Co 0.15 Mn 0.05 O2(NCM) was prepared. The LZO-coated cathode active material was manufactured according to the method disclosed in Korean Patent Publication No. 10-2016-0064942. Li6PS5Cl, an argyrodite-type crystal (D50 = 0.5 μm, crystalline), was prepared as a solid electrolyte. Polytetrafluoroethylene (PTFE) binder was prepared as a binder. Carbon nanofibers (CNF) were prepared as a conductive agent. These materials were mixed with a xylene solvent in a weight ratio of cathode active material: first two-dimensional solid electrolyte: amorphous particle-type solid electrolyte: conductive agent: binder = 84: 11.5: 3: 1.5, and the slurry was molded into a sheet shape, and then vacuum-dried at 40°C for 8 hours to manufacture a cathode sheet. The manufactured positive electrode sheet is placed on the carbon layer of the positive electrode current collector made of aluminum foil coated with a carbon layer on one side, and 85 o The positive electrode layer was manufactured by heated roll pressing of C. The total thickness of the positive electrode layer was about 120 ㎛. The thickness of each of the positive electrode active material layers was about 95 ㎛, and the thickness of the carbon-coated aluminum foil was about 25 ㎛. The initial charge capacity of the positive electrode layer (i.e., the positive electrode active material layer) was measured using the half-cell described above. The ratio (B / A) of the initial charge capacity (B) of the first negative electrode active material layer and the initial charge capacity (A) of the positive electrode active material layer was less than 0.5. The initial charge capacity of the positive electrode active material layer was measured at the first open circuit voltage (1 st4.25 V vs. Li / Li from open circuit voltage) + was determined by the charge up to . The initial charge capacity of the first negative active material layer was determined by the second open circuit voltage (2 nd 0.01 V vs. Li / Li from open circuit voltage) + It was determined by the charge up to .

[0326] (Manufacturing of solid electrolyte layer)

[0327] A mixture was prepared by adding 1.5 parts by weight of an acrylic binder to 98.5 parts by weight of the rGO (reduced graphene oxide)-Li6PS5Cl composite prepared in Manufacturing Example 1 as the first two-dimensional solid electrolyte. Octyl acetate was added to the prepared mixture and stirred to prepare a slurry. The prepared slurry was applied using a bar coater onto a 15 (m) thick nonwoven fabric placed on a 75 (m) thick PET substrate, and dried in air at 80°C for 10 minutes to obtain a laminate. The obtained laminate was vacuum-dried at 80°C for 2 hours. A solid electrolyte layer was prepared by the above process.

[0328] (All-solid-state secondary battery manufacturing)

[0329] An all-solid-state secondary battery was manufactured in the same manner as Example 1, except that the above-described positive electrode layer and solid electrolyte layer were used.

[0330]

[0331] Comparative Example 1: Mono-cell all-solid-state secondary battery, sulfide-based cathode active material (Li2S-C-LiI composite), flake solid electrolyte: particle-type solid electrolyte = 0:50 weight ratio

[0332] An all-solid-state secondary battery was manufactured in the same manner as Example 1, except that the weight ratio of the flake solid electrolyte and the particle solid electrolyte was changed to 0:50 and the flake solid electrolyte was not used.

[0333] Comparative Example 2: Mono-cell all-solid-state secondary battery, oxide-based cathode active material (NCA), flake solid electrolyte: particle-type solid electrolyte = 0:50 weight ratio

[0334] An all-solid-state secondary battery was manufactured in the same manner as Example 10, except that the weight ratio of the flake solid electrolyte and the particle solid electrolyte was changed to 0:50 and the flake solid electrolyte was not used.

[0335] Comparative Example 3: Mono-cell all-solid-state secondary battery, sulfide-based cathode active material (Li2S-C-LiI composite), using a simple mixture of rGO and Li6PS5Cl instead of a flake solid electrolyte (a composite of rGO and Li6PS5Cl).

[0336] An all-solid-state secondary battery was used in the same manner as in Example 1, except that a 1:60 weight ratio mixture of rGO and Li6PS5Cl was used instead of the flake solid electrolyte (a composite of rGO and Li6PS5Cl).

[0337] Comparative Example 4: Mono-cell all-solid-state secondary battery, oxide-based cathode active material (NCA), and a simple mixture of rGO and Li6PS5Cl instead of a flake solid electrolyte (a composite of rGO and Li6PS5Cl).

[0338] An all-solid-state secondary battery was used in the same manner as in Example 10, except that a 1:60 weight ratio mixture of rGO and Li6PS5Cl was used instead of the flake solid electrolyte (a complex of rGO and Li6PS5Cl).

[0339]

[0340] Reference Example 1: Sulfide-based cathode active material, inert material not used (free)

[0341] An all-solid-state secondary battery was manufactured in the same manner as Example 1, except that a flame-retardant inert material (i.e., a gasket) was not used during the manufacture of the all-solid-state secondary battery.

[0342] Reference Example 2: Oxide-based cathode active material, no inert material used (free)

[0343] An all-solid-state secondary battery was manufactured in the same manner as Example 10, except that a flame-retardant inert material (i.e., a gasket) was not used during the manufacture of the all-solid-state secondary battery.

[0344]

[0345] Example 12: One bi-cell all-solid-state secondary battery, sulfide-based cathode active material (Li2S-C-LiI composite), flake solid electrolyte: particle-like solid electrolyte = 10:40 weight ratio, first two-dimensional solid electrolyte

[0346] (Manufacturing of bi-cell all-solid-state secondary batteries)

[0347] The positive electrode layer was prepared in the same manner as in Example 1, except that the positive electrode active material layer was prepared to be arranged on both sides of the positive electrode current collector.

[0348] The total thickness of the positive electrode layer was approximately 220 μm. The thickness of each positive electrode active material layer was approximately 100 μm, and the thickness of the carbon-coated aluminum foil was approximately 20 μm.

[0349] The cathode layer, solid electrolyte layer, and flame-retardant inert member were each prepared in two pieces using the same method as Example 1.

[0350] Referring to Fig. 3, a solid electrolyte layer was placed on the negative electrode layer such that the first negative electrode active material layer was in contact with the solid electrolyte layer, and a positive electrode layer was placed on the solid electrolyte layer. The positive electrode layer had a structure in which positive electrode active material layers were placed on each side of the positive electrode current collector. A gasket was placed around the positive electrode layer to surround the positive electrode layer and to be in contact with the solid electrolyte layer. The thickness of the gasket was approximately 220 ㎛. The gasket may be, for example, a structure in which two gaskets having a thickness of 110 ㎛ are laminated or a single gasket having a thickness of 220 ㎛. The above-described flame-retardant inert material was used as the gasket.

[0351] The gasket was placed so as to contact the side surfaces of the anode layer and the solid electrolyte layer. The anode layer was placed in the center of the solid electrolyte layer, and the gasket was placed so as to surround the anode layer and extend to the ends of the solid electrolyte layer. The area of ​​the anode layer was approximately 90% of the area of ​​the solid electrolyte layer, and the gasket was placed over the entire area of ​​the remaining 10% of the solid electrolyte layer where the anode layer was not placed. The solid electrolyte layer was placed on the anode layer and the gasket, and the cathode layer was placed on the solid electrolyte layer to prepare a laminate.

[0352] 85 prepared laminates o C was plate pressed. This pressurization process sintered the solid electrolyte layer, thereby improving battery characteristics. The thickness of one sintered solid electrolyte layer was approximately 45 ㎛. The area of ​​the solid electrolyte layer was the same as that of the negative electrode layer. The pressed laminate was placed in a pouch and vacuum-sealed to manufacture an all-solid-state secondary battery. Part of the positive electrode current collector and negative electrode current collector were extended outside the sealed battery and used as positive electrode terminal and negative electrode terminal.

[0353]

[0354] Evaluation Example 1: High-temperature life characteristics test

[0355] The charge / discharge characteristics of the all-solid-state secondary batteries manufactured in Examples 1 to 9, Example 12, Comparative Example 1, Comparative Example 3, and Reference Example 1 were evaluated by the following charge / discharge test. The charge / discharge test was performed by placing the all-solid-state secondary batteries in a constant temperature bath at 45°C.

[0356] The first cycle is 0.6 mA / cm until the battery voltage is 2.5 V to 2.8 V. 2 The battery was charged for 12.5 hours at a constant current of 0.6 mA / cm until the battery voltage became 0.5 V. 2 Discharge was performed for 12.5 hours at a constant current.

[0357] The charge / discharge characteristics of the all-solid-state secondary batteries manufactured in Examples 10 to 11, Comparative Examples 2, 4, and Reference Example 2 were evaluated by the following charge / discharge test. The charge / discharge test was performed by placing the all-solid-state secondary batteries in a constant temperature bath at 45°C.

[0358] The first cycle is 0.6 mA / cm until the battery voltage is 3.9 V to 4.25 V. 2 The battery was charged for 12.5 hours at a constant current of 0.6 mA / cm until the battery voltage reached 2.5 V. 2 Discharge was performed for 12.5 hours at a constant current.

[0359] The discharge capacity of the first cycle was used as the standard capacity. From the second cycle onward, charging and discharging were performed up to 150 cycles under the same conditions as the first cycle. The measurement results are shown in Table 2 below.

[0360] The higher the number of cycles required for the discharge capacity to decrease to 95% of the standard capacity after the second cycle, the better the life characteristics were considered to be.

[0361] The all-solid-state secondary batteries of Reference Examples 1 and 2 suffered a short circuit before the first cycle was completed, making it impossible to measure life characteristics.

[0362] Number of cycles [times] Example 1 (mono-cell / Li2S-C-LiI complex + SE (flakes: particles = 10:40 weight ratio) / anode gasket / solid electrolyte layer (particle SE)) 500 Example 2 (mono-cell / Li2S-C-LiI complex + SE (flakes: particles = 5:45 weight ratio) / anode gasket / solid electrolyte layer (particle SE)) 410 Example 3 (mono-cell / Li2S-C-LiI complex + SE (flakes: particles = 20:20 weight ratio) / anode gasket / solid electrolyte layer (particle SE)) 300 Example 4 (mono-cell / Li2S-C-LiI complex + SE (flakes: particles = 30:20 weight ratio) / anode gasket / solid electrolyte layer (particle SE)) 200 Example 5 (mono-cell / Li2S-C-LiI complex+SE(flakes: particles=40:10 weight ratio) / anode gasket / solid electrolyte layer(particle SE))100Example 6 (mono-cell / Li2S-C-LiI-flake SE complex+SE(flakes: particles=10:40 weight ratio) / anode gasket / solid electrolyte layer(particle SE))600Example 7 (mono-cell / Li2S-C-LiI-flake SE complex+SE(flakes: particles=0:50 weight ratio) / anode gasket / solid electrolyte layer(particle SE))250Example 8 (mono-cell / Li2S-C-LiI complex+SE(flakes: particles=10:40 weight ratio), two-layer structure(top Example 9 (mono-cell / Li2S-C-LiI complex+SE (flake: particle = 10:40 weight ratio)) / anode gasket / solid electrolyte layer (particle SE))6502-layer structure (lower flake SE) / anode gasket / solid electrolyte layer (particle SE)) 550Example 10 (mono-cell / NCA+SE (flake: particle = 10:40 weight ratio) / anode gasket / solid electrolyte layer (particle SE)) 800Example 11 (mono-cell / NCA+SE (flake: particle = 0:50 weight ratio) / anode gasket / solid electrolyte layer (flake SE)) 700Example 12 (bi-cell structure / the rest is the same as Example 1) 600Comparative Example 1 (mono-cell / Li2S-C-LiI complex+SE (flake: particle = 0:50 weight ratio) / anode gasket / solid electrolyte layer (particle SE)) 210Comparative Example 2 (mono-cell / NCA+SE (flake: Particle phase = 0:50 weight ratio) / anode gasket / solid electrolyte layer (particle phase SE)) 400 Comparative example 3 (mono-cell / Li2S-C-LiI complex + SE (simple mixture of graphene and SE: particle phase = 10:40 weight ratio) / anode gasket / solid electrolyte layer (particle phase SE)) 180 Comparative example 4 (mono-cell / NCA + SE (simple mixture of graphene and SE: particle phase = 10:40 weight ratio) / anode gasket / solid electrolyte layer (particle phase SE)) 350,

[0363] As shown in Table 1, the all-solid-state secondary batteries including the sulfide-based positive electrode active materials of Examples 1 to 9 and Example 12 had improved life characteristics compared to the all-solid-state secondary batteries of Comparative Examples 1 and 3.

[0364] It was determined that the lithium batteries of Examples 1 to 9 had improved life characteristics by having an increased ion conduction path through the inclusion of a flake solid electrolyte and more effectively accommodating volume changes during charge and discharge of the positive electrode active material.

[0365] In the all-solid-state secondary batteries of Examples 1 to 5, the life characteristics varied depending on the weight ratio of the flake solid electrolyte and the particle solid electrolyte.

[0366] The all-solid-state secondary battery including the flake solid electrolyte of Example 1 exhibited improved life characteristics compared to the all-solid-state secondary battery of Comparative Example 3 including a simple mixture of graphene and solid electrolyte. It was determined that the simple mixture of graphene and solid electrolyte deteriorated the performance of the all-solid-state secondary battery due to increased side reactions caused by non-uniform mixing.

[0367] The all-solid-state secondary batteries including the oxide-based cathode active materials of Examples 10 to 11 had improved life characteristics compared to the all-solid-state secondary batteries of Comparative Examples 2 and 4.

[0368] It was determined that the all-solid-state secondary battery of Example 10 had an increased ion conduction path due to the arrangement of a flake solid electrolyte in the cathode active material layer, and had improved life characteristics by more effectively accommodating volume changes during charge and discharge of the cathode active material.

[0369] It was determined that the all-solid-state secondary battery of Example 11 had improved life characteristics by reducing the formation of pinholes on the surface of the solid electrolyte layer through the arrangement of a flake solid electrolyte on the solid electrolyte layer, thereby suppressing cracks in the solid electrolyte layer and resulting short circuits.

[0370] The all-solid-state secondary battery including the flake solid electrolyte of Example 10 exhibited improved life characteristics compared to the all-solid-state secondary battery of Comparative Example 4 including a simple mixture of graphene and solid electrolyte. It was determined that the simple mixture of graphene and solid electrolyte deteriorated the performance of the all-solid-state secondary battery due to increased side reactions caused by non-uniform mixing.

[0371] It was determined that the all-solid-state secondary battery of Example 12 has an improved lifespan characteristic by effectively alleviating volume changes during charge and discharge compared to the all-solid-state secondary batteries of Examples 1 to 5 having a mono-cell structure, since the battery has a bi-cell structure in which components are symmetrically arranged.

[0372] After the first cycle of charging was completed in the all-solid-state secondary batteries of Examples 1 to 12, SEM images of the cross-sections of these batteries were measured to confirm that a lithium metal precipitation layer corresponding to the second negative electrode active material layer was formed between the solid electrolyte layer and the negative electrode current collector.

[0373] As described above, the all-solid-state secondary battery related to the present embodiment can be applied to various portable devices, vehicles, etc.

[0374] While exemplary embodiments have been described in detail with reference to the attached drawings, the present invention is not limited to these examples. It is self-evident that those skilled in the art to which the present invention pertains can devise various modifications or variations within the scope of the technical concepts described in the patent claims, and these also naturally fall within the technical scope of the present invention.

[0375] [Explanation of symbols]

[0376] 1 All-solid-state secondary battery 10 Cathode layer

[0377] 11. Cathode current collector 12. Cathode active material layer

[0378] 20 Cathode layer 21 Cathode current collector

[0379] 22 First negative electrode active material layer 30 Solid electrolyte layer

[0380] 40 Inert Absences

[0381] 100 The first two-dimensional sulfide solid electrolyte

[0382] 110 cores 120 cores

[0383] 130 Middle Floor

[0384] 200 First two-dimensional sulfide-based solid electrolyte laminate

[0385] According to one aspect, it is possible to provide an all-solid-state secondary battery having a novel structure, in which short-circuiting is suppressed and cycle characteristics are improved.

Claims

1. It comprises an anode layer; a cathode layer; and a solid electrolyte layer between the anode layer and the cathode layer, The above positive electrode layer includes a positive electrode current collector and a positive electrode active material layer on at least one surface of the positive electrode current collector, At least one of the above cathode active material layer and the above solid electrolyte layer includes a first two-dimensional sulfide-based solid electrolyte, The above negative electrode layer includes a negative electrode current collector and a first negative electrode active material layer on one surface of the negative electrode current collector, An all-solid-state secondary battery, wherein the initial charge capacity (B) of the first negative electrode active material layer is less than about 50% of the initial charge capacity (A) of the positive electrode active material layer.

2. In the first paragraph, the first two-dimensional sulfide-based solid electrolyte is defined by length and thickness, The aspect ratio of the above length and thickness is approximately 3 or more, The length of the first two-dimensional sulfide-based solid electrolyte is about 1 to about 50 ㎛ and the thickness is about 10 nm to about 30 ㎛, An all-solid-state secondary battery, wherein the first two-dimensional sulfide-based solid electrolyte comprises a plate structure, a flake structure, or a combination thereof.

3. In the first paragraph, the surface of the first two-dimensional sulfide-based solid electrolyte has an irregular, circular or polygonal shape, An all-solid-state secondary battery, wherein the polygonal shape includes a triangle, square, pentagon, hexagon, heptagon, octagon, nonagon, or decagon.

4. In the first paragraph, the first two-dimensional sulfide-based solid electrolyte includes a core and a shell on the core, The above core includes a carbon-based material, a polymer, a metal-containing inorganic material, a sulfide-based solid electrolyte, an oxide-based solid electrolyte, or a combination thereof, The above shell comprises a sulfide-based solid electrolyte, an oxide-based solid electrolyte, a coating material, or a combination thereof, At least one of the above cores and shells comprises a sulfide-based solid electrolyte, The above core comprises a two-dimensional nanostructure, An all-solid-state secondary battery, wherein the two-dimensional nanostructure comprises graphene, graphene oxide, reduced graphene oxide, carbon nanobelt, carbon nanosheet, carbon nanoplate, carbon nanoflake, SiO2, TiO2, Al2O3, AlN, SiC, BaTiO3, or a combination thereof.

5. In the fourth paragraph, the ratio of the first thickness of the core and the second thickness of the shell is 1:0.01 to 1:1000, An all-solid-state secondary battery, wherein the ratio of the first length of the core to the second length of the shell is 1:1 to 1:

100.

6. In the first paragraph, the positive electrode active material layer includes a first region adjacent to the positive electrode current collector and a second region adjacent to the solid electrolyte layer, A first two-dimensional sulfide-based solid electrolyte is present in the first region and the first two-dimensional sulfide-based solid electrolyte is absent (free) in the second region, or A first two-dimensional sulfide-based solid electrolyte is present in the second region and the first two-dimensional sulfide-based solid electrolyte is absent (free) in the first region, or An all-solid-state secondary battery, wherein the first two-dimensional sulfide-based solid electrolyte exists in the first region and the second region.

7. In the first paragraph, the content of the first two-dimensional sulfide-based solid electrolyte is 1 to 50 wt% of the total weight of the positive electrode active material layer, The above cathode active material layer further includes a sulfide-based solid electrolyte of an irregular shape that is distinct from the first two-dimensional sulfide-based solid electrolyte, An all-solid-state secondary battery, wherein the weight ratio of the first two-dimensional sulfide-based solid electrolyte and the amorphous sulfide-based solid electrolyte is 1:99 to 99:

1.

8. In the first paragraph, the positive electrode active material layer includes a positive electrode active material, The above cathode active material includes an oxide-based cathode active material, a sulfide-based cathode active material, or a combination thereof, The above oxide-based cathode active material includes a lithium transition metal oxide, a metal oxide, or a combination thereof, and the lithium transition metal oxide includes lithium cobalt oxide, lithium nickel oxide, lithium nickel cobalt oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt mangense oxide, lithium manganate, lithium iron phosphate, or a combination thereof, and the lithium oxide includes iron oxide, vanadium oxide, or a combination thereof. An all-solid-state secondary battery, wherein the sulfide-based cathode active material comprises nickel sulfide, copper sulfide, Li2S, a Li2S-containing complex, or a combination thereof.

9. An all-solid-state secondary battery according to claim 8, wherein the Li2S-containing complex comprises a complex of Li2S and carbon, a complex of Li2S and carbon and a solid electrolyte, a complex of Li2S and a solid electrolyte, a complex of Li2S and a lithium salt, a complex of Li2S and a lithium salt and carbon, a complex of Li2S and a metal carbide, a complex of Li2S and carbon and a metal carbide, a complex of Li2S and a metal nitride, a complex of Li2S and carbon and a metal nitride, or a combination thereof.

10. In the 8th paragraph, the Li2S-containing complex further includes a second two-dimensional sulfide-based solid electrolyte, An all-solid-state secondary battery, wherein the size of the second two-dimensional sulfide-based solid electrolyte is smaller than the size of the first two-dimensional sulfide-based solid electrolyte.

11. In the first paragraph, the positive electrode active material layer further includes at least one selected from a conductive material and a binder, An all-solid-state secondary battery, wherein the conductive material comprises a carbon-based conductive material.

12. In the first paragraph, an inactive member is further included on one side of the anode layer, The above inert member surrounds the anode layer along the side of the anode layer, An all-solid-state secondary battery, wherein the inert member includes a position determining unit configured to determine the position of the inert member on the solid electrolyte layer.

13. An all-solid-state secondary battery, wherein the solid electrolyte layer comprises a first two-dimensional sulfide-based solid electrolyte arranged along one direction.

14. In the 13th paragraph, the first two-dimensional sulfide-based solid electrolyte is aligned in a direction substantially perpendicular to the thickness direction of the solid electrolyte layer, The above first two-dimensional sulfide-based solid electrolyte is laminated in the thickness direction of the solid electrolyte layer, An all-solid-state secondary battery, wherein the content of the first two-dimensional sulfide-based solid electrolyte is about 50 wt% or more of the total weight of the solid electrolyte layer.

15. In the first paragraph, the first negative electrode active material layer includes a negative electrode active material and a binder, An all-solid-state secondary battery, wherein the negative electrode active material has a particle form and the average particle diameter of the negative electrode active material is about 4 ㎛ or less.

16. In the 15th paragraph, the negative electrode active material includes at least one selected from a carbon-based negative electrode active material and a metal-based negative electrode active material, The above carbon-based negative electrode active material includes amorphous carbon, crystalline carbon, porous carbon, or a combination thereof. An all-solid-state secondary battery, wherein the metal-based negative electrode active material comprises gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), zinc (Zn), or a combination thereof.

17. In the 15th paragraph, the negative electrode active material comprises a mixture of first particles containing amorphous carbon and second particles containing metal, An all-solid-state secondary battery, wherein the content of the second particles is about 8 to about 60 wt% based on the total weight of the mixture.

18. In the 15th paragraph, the negative electrode active material comprises a carbon-based support; and a metal-based negative electrode active material supported on the carbon-based support, The above metal-based negative electrode active material includes a metal, a metal oxide, a complex of a metal and a metal oxide, or a combination thereof, The above metal-based negative electrode active material has a particle form, and the particle size of the metal-based negative electrode active material is about 1 nm to about 200 nm, An all-solid-state secondary battery, wherein the carbon-based support has a particle shape and the particle size of the carbonaceous material is about 10 nm to about 2 ㎛.

19. In the first paragraph, a second negative electrode active material layer is further included between the solid electrolyte layer and the negative electrode current collector, The second negative electrode active material layer is at least one of between the first negative electrode active material layer and the first protective layer and between the first negative electrode active material layer and the solid electrolyte layer, An all-solid-state secondary battery, wherein the second negative electrode active material layer is a metal layer containing lithium metal or a lithium alloy.

20. In the first paragraph, at least one of the positive electrode current collector and the negative electrode current collector includes a base film and a metal layer on at least one surface of the base film, The above base film comprises a polymer, and the polymer comprises polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI) or a combination thereof, An all-solid-state secondary battery, wherein the metal layer comprises indium (In), copper (Cu), magnesium (Mg), titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.

Citation Information

Patent Citations

  • Cathode for lithium ion secondary battery, and lithium ion secondary battery

    KR1020160064942A

  • Composite material and preparation method thereof, solid-state battery and electric equipment

    CN115117434A

  • Solid electrolyte particle, solid electrolyte membrane and method for producing solid electrolyte particle

    JP2013058376A

  • Negative active material for lithium secondary batteryand method of preparing same

    KR1020060103031A

  • A structure of complexed cathode using Li2S

    KR1020150131652A

Cited By

  • Use of microbiome and metabolomic clusters for evaluating skin health

    RU2846741C1