Inert media enhanced catalytic pyrolysis of hydrocarbons

WO2024206754A3PCT designated stage expired Publication Date: 2024-11-21RGT UNIV OF CALIFORNIA
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/US2024/022140
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-29
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Current pyrolysis methods for producing hydrogen from hydrocarbons require high temperatures and result in carbon products contaminated with polycyclic hydrocarbons, and there are no significant commercial processes using pyrolysis to produce hydrogen as a primary product due to catalyst deactivation and high-cost catalysts.

Method used

A fluidized bed reactor system using a mixture of catalyst particles and inert particles with different densities, allowing for stratification and selective heating, which facilitates hydrogen production at lower temperatures and prevents carbon contamination by physically reactivating the catalysts and removing carbon deposits.

Benefits of technology

The system achieves high yields of hydrogen and carbon per unit mass of catalyst at lower temperatures, with the inert particles enabling efficient heat transfer and catalyst reactivation, reducing catalyst deactivation and carbon contamination, and allowing for cost-effective hydrogen production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2024022140_21112024_PF_FP_ABST
    Figure US2024022140_21112024_PF_FP_ABST
Patent Text Reader

Abstract

A system for converting hydrocarbons gases to solid carbon and hydrogen products includes a pyrolysis reactor comprising a bed of particulates, and a separator in fluid communication with the pyrolysis reactor through the product gas outlet. The bed of particulates includes catalyst particles, solid carbon, and inert particles, and the pyrolysis reactor has a feed gas inlet at a lower portion of the bed of particulates, and a product gas and solid outlet above the bed of particulates. The separator is configured to separate any particulates in a product gas produced in the pyrolysis reactor.
Need to check novelty before this filing date? Find Prior Art

Description

INERT MEDIA ENHANCED CATALYTIC PYROLYSIS OF HYDROCARBONS CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] The present application claims priority (under 35 U.S.C. Section 119(e)) to U.S. Provisional Application 63 / 493,489 filed on March 31, 2023 and entitled “INERT MEDIA ENHANCED CATALYTIC PYROLYSIS OF HYDROCARBONS,” which application is incorporated herein by reference in its entirety. STATEMENT REGARDING GOVERNMENTALLY SPONSORED RESEARCH OR DEVELOPMENT

[0002] None. BACKGROUND

[0003] The pyrolysis of low-cost hydrocarbon feedstocks including petroleum and natural gas produces solid carbon and gas phase molecular hydrogen. For example, the conversion can occur according to the following equation: ^(CH2m) ^ ^ ^ Csolid^mH2

[0004] This reaction has the potential for producing a hydrogen product without carbon dioxide which is a major challenge in society today. In the absence of a catalyst, the reaction requires very high temperatures (T >1000 °C) and there are many technical challenges associated with heat management in such high temperature processes. Further, the carbon product produced is typically associated with polycyclic hydrocarbon contaminants. To date there have been no significant commercial processes using pyrolysis to produce hydrogen as a primary product.SUMMARY

[0005] In some embodiments, a system for converting hydrocarbons gases to solid carbon and hydrogen products comprises a pyrolysis reactor comprising a bed of particulates that comprises catalyst particles, solid carbon, and inert particles, and a separator in fluid communication with the pyrolysis reactor through the product gas outlet. The pyrolysis reactor comprises a feed gas inlet at a lower portion of the bed of particulates, and a product gas and solid outlet above the bed of particulates. The separator is configured to separate any particulates in a product gas produced in the pyrolysis reactor.

[0006] In some embodiments, a fluidized bed reaction process comprises contacting a hydrocarbon reactant with a fluidized bed within a reactor, stratifying the fluidized bed within the reactor, forming the solid carbon and hydrogen based on contacting the hydrocarbon reactant with the fluidized bed, and removing the hydrogen and at least a portion of the solid carbon from the reactor. The fluidized bed comprises catalyst particles, solid carbon, and inert particles, and the inert particles move to a lower portion of the fluidized bed. The solid carbon and catalyst particles move to an upper portion of the fluidized bed.

[0007] In some embodiments, a fluidized bed reaction process comprises contacting a hydrocarbon reactant with a fluidized bed within a reactor, stratifying the fluidized bed within the reactor, forming the solid carbon and hydrogen based on contacting the hydrocarbon reactant with the fluidized bed, reacting at least a portion of the impurity with a portion of the catalyst particles, and removing the hydrogen and at least a portion of the solid carbon from the reactor. The fluidized bed comprises catalyst particles, solid carbon, and inert particles, and the hydrocarbon reactant comprises an impurity. The inert particles move to a lower portion of the fluidized bed, and the solid carbon and catalyst particles move to an upper portion of the fluidized bed during the contacting.BRIEF DESCRIPTION OF THE DRAWINGS

[0008] For a more complete understanding of the present disclosure, reference is now made to the following brief description, taken in connection with the accompanying drawings and detailed description:

[0009] Figure 1 illustrates micrographs and Raman spectroscopy results for carbon produced with and without the addition of a catalyst.

[0010] Figures 2A and 2B illustrate block diagrams of a fluidized bed with external heating with and without heat integration according to some embodiments.

[0011] Figure 3 illustrates photographs of a catalyst bed with and without sand.

[0012] Figure 4 schematically illustrates a fluidized bed with and without inert particles included with the catalyst.

[0013] Figures 5 schematically illustrates another fluidized bed with heat integration and external heating according to some embodiments.

[0014] Figure 6A schematically illustrates the process of forming catalyst particles from catalyst precursors according to some embodiments.

[0015] Figure 6B illustrates the formation of catalyst particles from catalyst precursors within the fluidized bed according to some embodiments.

[0016] Figure 6C illustrates the X-ray diffraction from carbon on iron ore and iron catalysts.

[0017] Figure 6D illustrates images of the carbon formed from catalyst particles according to some embodiments.

[0018] Figure 7 schematically illustrates another fluidized bed with heat integration and external heating according to some embodiments.

[0019] Figure 8 schematically illustrates fluidized bed reactors with external heating and heat integration according to some embodiments.

[0020] Figure 9 schematically illustrates a fluidized bed with internal heating with and without heat integration according to some embodiments.

[0021] Figure 10 schematically illustrates a fluidized bed with internal heating and heat integration according to some embodiments.

[0022] Figure 11 schematically illustrates the stratification of the bed within a fluidized bed reactor according to some embodiments.

[0023] Figure 12 schematically illustrates the transformation and fragmentation of a macroscopic solid catalyst precursor into active catalyst nanoparticulates according to some embodiments.

[0024] Figure 13 is experimental data as described in specific examples.

[0025] Figure 14 is experimental data as described in specific examples.

[0026] Figure 15 is experimental data as described in specific examples.

[0027] Figure 16 is experimental data as described in specific examples.

[0028] Figure 17 is experimental data as described in specific examples.

[0029] Figure 18 is experimental data as described in specific examples.

[0030] Figure 19 is experimental data as described in specific examples. DETAILED DESCRIPTION

[0031] The processes, systems, and methods disclosed herein demonstrate how molecular hydrogen production from the decomposition of hydrocarbon feedstocks can be facilitated by the novel combination of catalytic materials for methane decomposition and chemically inert materials and the synergistic interactions between the catalytic and inert particles in fluidized bed reactors. The physical interactions between the inert and catalytic solids provides for high yields of hydrogen and carbon per unit mass of catalyst, and the significant density difference between the inert solid and catalyst adherent to the nanometer scale catalyst allows for a stratification of the solids within the reactor and efficient heat transfer. Use of the inert material in the novel reactor design allows for stratification and selective circulation of inert particles to allow for heat addition. The preferred transition metal catalysts are active allowing for relatively low reaction temperatures and sufficiently low-cost and safe to allow for low-cost carbon management.

[0032] To facilitate the reaction at lower temperatures, catalysts have been used including transition metals (e.g. Fe, Ni, Co). Certain carbons have also been shown to bea moderately active catalyst for pyrolysis. Catalytic pyrolysis of methane has been observed at temperatures as low as 600 °C on transition metals which are the most active pyrolysis catalysts. In general, solid catalysts used for pyrolysis in fixed bed reactors rapidly deactivate as the solid carbon is deposited on the catalyst surface, thereby blocking access to the catalytic sites by the hydrocarbon. Provided sufficient hydrogen can be produced prior to catalyst deactivation, it is possible to make use of catalysts in a process that either regenerates the catalyst activity or disposes of the catalyst together with the solid carbon. n(CH2m) ^Active Catalyst ^ ^ ^ nCsolid^ n* mH2^ Inactive Catalyst

[0033] If the catalyst can be replaced or regenerated at a very low cost and the hydrogen yield per unit mass of catalyst is sufficiently high such a process might be cost-effective. Typically, the carbon (coke) can be removed by oxidation to regenerate the catalyst which produces unwanted carbon dioxide. To date, only iron has been found to have sufficiently low-cost and high hydrogen yields to be of potential use in the pyrolysis of hydrocarbons.

[0034] Fluidized bed reactors (FBR) for methane pyrolysis using iron catalysts have been previously investigated and disclosed. Prior work with iron in FBR for pyrolysis using Fe and Fe supported on alumina was shown to be highly active at 1000 ℃, however, rapid deactivation was observed [1]. Torres et al. investigated methane decomposition in fluidized bed reactor with Fe / Al2O3in the temperature range of 700-900 ℃ and space velocities between 3-6 L / gcat.h and achieved 40% conversion up to 6 h with 4.8 grams of carbon per gram of catalyst [2]. They also observed that conversion increases by increasing temperature and lowering space velocity. Additionally, the deposited carbon was in the form of nanofibers and multiwall nanotubes. Similar work in a fluidized bed at 850 ℃ with spray coatings of iron oxide on alumina showed high initial activities with decreasing activity as the C:Fe mole ratio increased beyond 2 [3]. Similarly, iron oxide coated zirconia was used in a fluid bed at approximately 800 ℃ showed high initial activity with a rapid deactivation [4]. Qian et al. proposed a fluidized bed with 40% Fe on Alumina at 750 ℃ was reported to have a conversion of over 75% for an hour and achieved 11 gms C per gm of catalyst [5]. The same research work also explored the ironore as a catalyst in fluidized bed reactor for methane pyrolysis and achieved 60% methane conversion up to 5 h 850 ℃, 5 bar and 3.75 L / gcat.h [6]. Further, they explored the iron concentrated powder, fine / coarse ash and steel slag, volcanic mud powder as a catalyst for methane pyrolysis [7]. Among all these, iron concentrated powder was found to be best suitable candidate for methane pyrolysis and achieved 4.7 gms C per gm of catalysts at 3 L / gcat.h space velocity and 900 ℃. The major innovation of the present systems and methods over prior art is the intermixing of physically separate (e.g., not supported) components of iron catalyst and a dense inert component which provides both physical interactions between the catalyst to facilitate re-activation and dislodgement of carbon, and the stratification of the fluidized bed to allow the selective removal of the inert phase material to be separately contacted for heating.

[0035] Recently, Siriwardane and co-workers proposed iron alumina catalysts in fluidized bed reactor for methane decomposition and attained stable 80% conversion up to 160 h and remained above 60% up to 225 h at 700 ℃ and thereafter declined rapidly [8]. However, the maximum C / Fe ratio was limited to approximately ~4 grams carbon per gram of catalyst. High activity could be attributed to the high catalyst loading (500 g catalyst) and low space velocity (10% CH4at 0.396L / gcat.h).

[0036] US 2012 / 02583.74 A1 discloses the process to produce hydrogen and graphite particles from light hydrocarbons using calcined iron containing catalyst or bimetallic MxNiy-type supported catalysts in the temperature range of 650 to 1200 ℃. The method shows a catalytic conversion efficiency in the range of 0.3 to 0.95. Typically, greater than 0.4 at temperature 800 ℃ or higher up to 50 h. It also considered the apparatus for generating electricity which consists a catalytic reactor, a separator and a fuel cell to generate electricity.

[0037] WO 2020 / 121287 discusses a method of producing pure hydrogen and carbon through catalytic methane decomposition using electrochemical, membrane, or a packed bed or fluidized bed reactor at low temperature. The reference further discloses the process of removing accumulated carbon from the catalyst surface. The regeneration method discloses that the carbon can be detached from the surface of carbon particle byfeeding small fraction of produced hydrogen back to reactor for converting carbon at an interface of catalyst to methane.

[0038] US 7,001,586 B2 discusses a process for CO free hydrogen through methane decomposition using NixMgyO and NixMgyCu2O in the temperature range to 425 ℃ to 625 ℃. It also reveals a method of synthesizing these catalysts through multi-step thermal crystallization process.

[0039] US 2008 / 0210908 A1 discusses a process to produce hydrogen enriched fuel and carbon nanotubes using microwave irradiation in the presence of metal catalysts. The product gas consists the higher hydrocarbons such as C2H4, C2H2, C3H6, C3H8and others due to microwave plasma assisted methane decomposition.

[0040] Patrianakos et al. examined the influence of carbon as a seed particle to facilitate methane conversion and carbon black formation in solar thermal reactors. They found that the 80 g / min carbon seed addition in methane flow rate at 600 g / min resulted in 10- 15% carbon deposition on wall of reactor and remaining ~85% carbon nucleated in the gas phase in a 80 mm ID tube at 1600 ℃ and equilibrium conversion. [9] They further concluded that the seeding in the reactor at high temperature only increased the heat transfer rate. Seeding does not play any role in methane conversion and carbon formation.

[0041] The major challenges of handling of iron-based catalysts in fluidized bed reactor are agglomeration and sintering of iron particles in presence of reducing environment at elevated temperature, formation of unwanted carbon byproducts, and the separation and high density of iron particles still remain unresolved. Further, most prior work relied on first processing the iron or other metal at significant cost and fabricating specific supported catalysts to achieve activity. In order to solve these issues, the use of iron in a fluidized bed reactor can be used with specific process and design considerations. These challenges are solved by the present systems and methods.

[0042] In all prior art systems with metal catalysts, the hydrogen yield per unit mass of the relatively expensive catalyst has been relatively low and the opportunities for heat addition limited. The novel aspects of the invention described herein make use of the cooperative interaction of inert particles which are relatively dense compared to thecarbon product produced on the surface of metal-based catalysts. These interactions allow for greater yields of hydrogen and carbon per unit mass of catalysts and the properties of the inert allow for stratification of the inert particles within the reactor and selective removal and / or heating of the inert particles. The physical interactions of the inert particles with the catalysts within the fluidized bed physically reactivate the catalysts by attrition which helps to disengage the carbon from the catalyst allowing additional reaction activity and greater yields.

[0043] The systems and methods disclosed herein provides a means for utilization of a catalyst for methane pyrolysis and reactor systems for its use that provide for high hydrogen yields at modest temperatures with a low-cost catalyst. The invention makes use of a fluidized bed containing a mixture of catalysts, carbon, and inert particles with different densities and sizes which allow for unique stratification and segregation behavior within the fluidized reactor bed. This behavior, by design, facilitates both heat transfer to the reactor, high utilization of the catalyst, and carbon product removal.

[0044] The novel combination of an inert solid with an active catalyst makes use of the fluidized inert solid in part to physically reactivate the catalyst within the fluidized bed to maximize the hydrogen yield per kg of catalyst added to the reactor. Further, in some embodiments, heat addition can be supplied by high temperature combustion gases applied directly to the inert particles which, because of their density segregation, can be continuously removed without the presence of significant quantities of solid carbon containing the catalyst.

[0045] In some aspects, a reactor is disclosed in which there are two or more different types of solids, at least one of which is chemically inert. By introduction of the denser and / or larger solid particles at the top of the reactor, a countercurrent movement of inert particles can be established where the inert particles are utilized for energy transfer and for physical interactions with the lower density active components (catalyst precursors and catalysts) which enable the unique production of specific chemical products. The inert particles can be a relatively low cost means of carrying energy into reactors producing or requiring heat. In addition to the use for hydrocarbon pyrolysis wherebycountercurrent movement of high temperature insulating solids (e.g. sand) brings heat into the reactor to allow low density carbon to be produced and exit at the top of the reactor, other important applications are also envisioned and enabled. For example, in catalytic hydrocarbon reforming, typically expensive tubular packed bed reactors are utilized and contaminant free feedstocks is required. A countercurrent fluidized bed of a heated dense downward moving solid (e.g. sand) intermixed with a lower density reforming catalyst (e.g. metal on low density support) would allow fluidized bed reforming of otherwise undesirable feeds. For example, the proper selection of catalyst and particle sizes can be used to establish a stratified bed having inert particles in a lower portion, a potential guard bed of particles in the middle, and additional or different catalytic particles at the top, where the guard bed can be used to react with contaminants prior to reaction of the reactants with the catalytic particles at the top.

[0046] In some aspects, the processes described herein can be used for pyrolysis reactions. The unique feature of the hydrocarbon pyrolysis reaction occurring in contact with a catalyst such as iron can be compared to the reaction occurring on an inert (e.g., sand). The carbon produced can have different morphologies, which is shown in Figure 1. At 1200 °C, carbon can be produced in a fluidized bed reactor using an inert alone such as sand. However, as shown in the upper left micrograph, the resulting low-density carbon is disordered as also shown in the Raman spectra which shows broad D and G peaks characteristic of sooty carbon. The carbon product obtained at 1200 °C also can have significant fractions of undesirable polycyclic hydrocarbons. At 950 °C, methane does not react on sand, however, it does react with an iron-based catalyst to produce graphitic carbon as can be seen in the lower left micrograph and Raman spectrum which shows a dominant sharp G peak consistent with graphitic carbon. This carbon has no or substantially no undesirable polycyclic hydrocarbons present. Similar graphitic carbon can be produced with any of the catalysts described herein, which can be distinct from pyrolysis occurring on inert materials alone that produce non-graphitic carbon.

[0047] An embodiment of a process is represented schematically in Figure 2A whereby the hydrocarbon feedstock 10 can be preheated and introduced into the bottom of thefluidized bed reactor 20 containing a mixture of catalyst (e.g., catalytic particles) and an inert solid. While shown as being methane, the hydrocarbon feedstock 10 can comprise any suitable hydrocarbon, including but not limited to, light alkanes such as methane, ethane, natural gas, alkenes, alcohols, as well as other gaseous hydrocarbons, including those that can be gasified such as the gasified or pyrolyzed products of liquid, and solid hydrocarbons (e.g. crude oil, biomass, naphtha, etc.). The hydrocarbon can travel upward in the reactor, and upon contacting the catalyst, produces solid carbon and gas phase hydrogen. The catalyst and carbon are generally partially adherent, and due to the relatively low density of the carbon / catalyst solid relative to the inert particles, move towards the top of the solids bed in the reactor 20 under the influence of the upward moving gases. Heated inert particles 30 can be introduced at or near the top of the reactor 20 and due to their size and density travel downward, countercurrent to the rising gases and solid carbon / catalyst. The heated inert particles can continue to move downwards and contact the hydrocarbon feed, bringing the feed to reaction temperatures to allow the pyrolysis reaction to occur upon contact with the catalyst. The temperature within the reactor 20 can be maintained below the reaction temperature of the hydrocarbon with the inert solid (e.g., below a non-catalytic pyrolysis temperate).

[0048] Within this process, the catalyst can comprise any suitable catalyst used for the desired reaction. In some aspects, the catalyst can exhibit catalytic activity towards hydrocarbon pyrolysis. Suitable pyrolysis catalysts can comprise iron, nickel, manganese, cobalt, oxides thereof, and / or salts thereof. In some aspects, relatively low value oxide ores may be provided to the fluidized bed reactor, and within the pyrolysis environment, the oxide ores are reduced and fragmented into nanoparticulate catalysts comprised of metallic and / or metal carbide character.

[0049] When the catalyst comprises iron, the catalyst can exist primarily as iron carbide, Fe3C, due to the reducing carbon-rich environment within the reactor 22. The precursors, including but not limited to particulates of iron ore, pig iron, and iron that typically have sizes between 10 and 1000 micrometers (µm) can be introduced into the fluid bed reactor and interact with the hydrocarbon and hydrogen reactor environment where any ironoxides are reduced to metallic iron which in the presence of a hydrocarbon becomes a mixture of metallic iron and iron carbide. The solid matrix of the catalyst can be altered during the transformation which allows the fracturing of the macroscopic micron size particles into smaller nanometer size particulates facilitated by the mechanical collisions with the inert solid. The active catalyst particles, once reduced in size, can typical sizes between about 1 and 1000 nanometers (nm).

[0050] In some embodiments, one or more promotors, dopants, or other elements can be used with the catalyst. Another unique aspect of the systems and methods disclosed herein is the addition of additives or conditions that enable the catalyst to be activated or “promoted” for a desirable reaction. In general, Lewis base metals (alkali’s) or Lewis acids (Halogens) can change the activity of metal catalysts. For example, if a metal oxide were the catalyst precursor for a reaction with methane, the iron oxide could be mixed with an alkali metal nitrate (e.g. nitrates of potassium, sodium, calcium, magnesium) to promote the reactions on iron. In the example of KNO3 in the high temperature environment the iron catalyst would be contacted with K as a promoted Fe(K) catalyst. Low cost alkali chloride salts may also be added (NaCl, KCl, MgCl2, and CaCl2, might all be used and the catalysts heated within the reactors. Halogen promotion might also be accomplished through introduction of hydrogen halides, alkylhalides, or halogens themselves. Any such catalyst activations and promotions can be used with the catalysts described herein.

[0051] The inert particles or particles can comprise any suitable inert material that is stable at the reaction temperatures and conditions. For example, any suitable oxides or ceramics can be used. In some aspects, the inert particles can be formed from sand, gravel, magnesia, alumina, zirconia, or any other suitable inert materials. The initial size of the inert particles can be within the micrometer to millimeter size ranges. For example, the inert particles can have a size in a range of between about 0.01 to about 10 mm. In some aspects, the inert particles can have a range of sizes or be selected to be within a narrow size range. The size of the inert particles can be selected based on the expected operating conditions (e.g., gas flow rates, temperature, etc.) of the reactor. While someattrition of the inert particles may occur over time, the inert particles may be expected to remain relatively stable within the reactor as compared to the starting materials for the catalyst or catalyst precursors within the reactor. At the stable operating conditions, the ratio of the diameter of the active catalyst particles to the diameter of the inert particles can be in the range of about 1:10 to about 1:10,000, or between about 1:100 to about 1:1,000.

[0052] Within the reactor, the combination of the catalyst particles (e.g., both catalyst precursors and active catalyst particles) with the inert particles can be used during the reaction. Within the catalyst bed, the catalyst particles can be present and make up at least about 1 wt.%, at least about 10 wt.%, at least about 20 wt.%, or at least about 25 wt.% of the overall particles present in the bed, and the catalyst particles may be less than about 90 wt.%, less than about 75 wt.%, less than about 70 wt.%, or less than about 40 wt.% of the overall particles present in the bed.

[0053] The reaction can take place in a reactor as shown schematically in Figure 2A (and as otherwise described herein) can take place with a temperature between about 400- 1200 °C, between about 500-1100 °C, or between about 600-1000 °C. The hydrocarbon gas can have a residence time of at least about 0.01, at least about 0.1, at least about 0.3, or at least about 0.5 seconds, where the residence time refers to the time the hydrocarbon gas is in contact with the particle bed. In some aspects, the hydrocarbon gas can have residence time of less than about 10 seconds, less than about 7 seconds, or less than about 5 seconds. In a preferred embodiment the gas residence time is between 0.5 and 3 seconds. The resulting solid carbon formed can have a carbon to iron weight ratio (e.g., C / Fe ratio) of greater than about 5, greater than about 7, greater than about 10, greater than about 15, or greater than about 20. The reaction can occur at a pressure between about 0.1 bar and about 30 bar, or between about 1 to 10 bar.

[0054] To improve the thermal efficiency of the process, the lower section of the reactor containing primarily inert particles can be extended, as shown in Figure 2B, to allow the lower temperature hydrocarbon feed 10 to contact the fluidized inert particles, which heats the hydrocarbon feed 10 and cools the inert particles. The lower temperature of thereactor bed can be contacted with heat exchange surfaces 40, allowing a thermal fluid to be cooled by the hydrocarbon feed. The thermal fluid can be circulated and allowed to exchange heat using upper heat exchange surfaces 42 with the product stream exiting the reactor, thereby cooling the exit stream and heating the thermal fluid which can be returned to the lower section of the reactor; thus providing near ideal heat integration.

[0055] The heat integration using the heat exchange surfaces can use any suitable heat exchange fluid. For example, gasses, molten salts, molten metals, or other high temperature heat exchange fluids can be used. In some aspects, the heat exchange surfaces 40 may be electrically heated, combustion heated, or the like. For example, renewable electricity can be used to heat the lower heat exchange surfaces 40 to heat the hydrocarbon feed 10. In other examples, electricity from renewable energy sources such as solar cells or wind turbines can be used to heat a large insulated reservoir of inert material from which the circulating solids for the reactor can be drawn.

[0056] In some embodiments, the heat integration and / or heat source (e.g., in the heating section) can use concentrated solar energy to provide the heat for the pyrolysis reactor. Solar concentrators harness heat from the sun, whereby solar energy is focused using mirrors on a heat transfer surface and the thermal energy can be transferred into a heat transfer media. In some embodiments, the solar heat can be concentrated on the circulating solid inert material where it is heated to temperatures between 700 °C and 1100 °C. The solar energy input can take place outside of the reactor such as in a heating section. The heated, solid inert particles can then be circulated into the pyrolysis reactor as described herein. In some embodiments, a heat transfer fluid can be heated using solar energy and passed to heat transfer surfaces within the reactor to transfer heat into the reactor, for example, at an upper and / or lower portion of the reactor.

[0057] Apart from stratification, addition of an inert material also allows the maintenance and balancing of both a sufficiently long residence time (for reaction) without mass transfer limitations at high space velocity (for fluidization) while maintaining an improved or optimized iron loading. In principle, the residence time (e.g., the time the gas requires to move through the catalyst bed) decreases by increasing thespace velocity. The higher the space velocity, the shorter the residence time which can result in lower conversion due to less chance of collisions between the hydrocarbon molecules (e.g., CH4, etc.) and iron particles as shown in Figure 12. Further, the mass transfer limitation due to the very high volumetric reaction rate (moles / m3-s) limits the maximum rate. By the addition of sand to a given amount of iron, the gas residence time can be increased within the bed several order of magnitude, for example from a few milliseconds to a few seconds at the same space velocity. The longer residence time allows for a greater chance of collisions between the reactants and a catalyst surface without the mass transfer limit.

[0058] As an example, 28 g of sand and iron with 20% iron (5.6 g of Fe) has a 14 cm bed height in a 1.4 cm diameter tube. However, 5.6 g of Fe without sand has only 1.8 cm bed height in a 1.4 cm diameter tube which resulted into very low residence time (under mass transfer limited conditions) which could compromise the observed activity. Figure 3 shows the same amount of iron in both tubes (5.6 g) but different bed heights which resulted into difference in their respective space velocities and residence time. As an exemplary set of reaction conditions, at 950℃, 240 ml / min as the residence time of 1.3 sec in the case of 20% iron. However, in the case of pure iron the residence time is just few milliseconds. The reactor cost can be increased due to the greater reaction volume, however, the benefits in conversion, stratification, operability, and the physical interactions between the inert particles and the catalyst can outweigh the potentially greater reactor size and cost.

[0059] Another embodiment of a reactor system is shown schematically in Figure 4. As shown, methane or other hydrocarbon gases making up the hydrocarbon feed 10 can be preheated and introduced into a lower portion of the reactor 22, which can comprise a fluidized bed reactor in some embodiments. By virtue of their density, the inert particles can be segregated to the bottom section of the reactor 22 where they contact the relatively low temperature hydrocarbon feed 10, thereby pre-heating the hydrocarbon feed 10 as it rises into the main section of the reactor 22. Within the main section, the hydrocarbon feed 10 contact the iron catalyst within the bed of solids, including the catalytic particles,solid carbon, and inert particles. When the catalyst comprises iron, the catalyst can exist primarily as iron carbide, Fe3C, due to the reducing and carbon containing environment within the reactor 22. The pyrolysis reaction can occur as the hydrocarbon rises in the bed to produce hydrogen and solid carbon. The freeboard (e.g., the headspace in the reactor that is not loaded with particles or solids) of the reactor 22 can be designed such that as the low-density carbon containing trace amounts of the catalyst such as iron accumulates, a fraction of the solids can exit the reactor 22 with the hydrogen and be separated from the hydrogen using a separator 42 such as a cyclone and / or filter. In other embodiments, the solids can be withdrawn from the top of the bed as they accumulate through an optional dedicated solids transfer line 44. In some aspects, the solids can be removed from any portion of the reactor such as the portion of the bed where the carbon accumulates during the reaction process.

[0060] The dense inert particles that accumulate at the bottom of the reactor 22 can be withdrawn through an outlet and moved to a heating section 46 whereby the inert particles can be contacted and lifted in a riser with high temperature gas generated by a number of possible means including by hydrocarbon or hydrogen combustion or electric heating. A loop seal or other valveless unit for solid transport can be used at the outlet of the inert particles to allow for the removal of the inert particles from the reactor 22 while preventing the outflow or backflow of gases into the reactor. The inert particles can be heated in the heating section 46, transported, and then separated from the heating gas in a separator 48 such as a cyclone. The hot inert particles can then be returned to the main reactor 22 through a loop seal or other valveless unit for solid transport that prevent undesired gas contacting. The inert particles can move downward within the reactor 22 solids bed countercurrent to the rising less-dense carbon contain catalyst, where heat can be supplied for the reaction through contact of the hot inert particles with the catalyst, carbon, and hydrocarbon gases. An element of the systems and methods is the intermingling of the hot inert particles with the catalyst within the solid fluidized bed whereby heat transfer is achieved and attrition of the carbon from the iron catalyst canprovide for continual reactivation of the catalytic surface through physical contact between the inert particles and the active catalytic phases.

[0061] To maintain a constant steady-state inventory of active catalyst within the reactor 22, additional catalyst or catalyst precursors can be added to the reactor at one or more locations. In some aspects, the catalyst can be added directly into the reactor 22. As described herein, any metal oxides present may be reduced to the metallic or carbide forms within the reactor. If the catalyst is added to inert particles in the side leg or heating section, the metals may oxidized to form metal oxides. Upon entering the reactor 22, the metal oxides may be reduced to metallic or carbide forms, along with some amount of carbon oxides. The addition of the catalyst directly into the reactor 22 (e.g., at the top or within the particle bed) may be used to avoid the formation of any carbon oxides in the system, but the catalyst can also be added in other locations as desired to operate the system.

[0062] The use of the density stratified fluidized bed brings the inert particles to the bottom of the bed and allows for facilitated heat integration between the hot gas exiting the reactor and the inlet hydrocarbon feed. One of several implementations is shown schematically in Figure 5. The hot product gas at the top of the reactor can be cooled by heat exchange surfaces 42 in the freeboard above the particle bed, which can exchange heat with the inert particles at the bottom of the fluid bed using heat exchange surfaces 40. For example, hot product gasses at approximately 950 °C can be cooled and the heat can be exchanged with the inert particles at the bottom of the fluid bed where relatively cool hydrocarbons in the hydrocarbon feed at approximately 500 °C can be fed. The heat exchange heats the inert particles at the reactor bottom. Although there will likely be modest reactivity with the hydrocarbon feed, the fluidized inert particles will prevent any accumulation of carbon, and attrition can disengage any carbon formed on the inert particle surfaces to allow the low-density carbonaceous product to be lifted into the hotter reactor sections above. Depending on the heat source used in the heating section 46, any remaining carbon on the surface of the inert particles may be oxidized to remove thecarbon from the surface of the inert particles prior to returning the hot inert particles to the top of the particle bed.

[0063] An element of the system and methods disclosed herein is the synergistic interaction of the inert particles with the active solid catalyst. Figure 6A schematically illustrates the transformation of a number of solid catalyst precursors within the reactor into active pyrolysis catalysts. The precursors, including but not limited to particulates of iron ore, pig iron, and iron can be reduced to metallic iron and a metal carbide within the reactor. The solid matrix of the catalyst can be altered during the transformation which allows the fracturing of the macroscopic micron size particles into smaller nanometer size particulates facilitated by the mechanical collisions with the inert solid. The high surface area nanoparticles of iron / iron carbide interact with gas phase methane producing hydrogen and carbon formed in graphitic and / or filamentous structures from the surface of the solid catalyst. The carbon formed from the catalyst surface can be free of contaminants such as polycyclic hydrocarbons and can be predominately of graphitic character.

[0064] Based on the atmosphere of the reactor, raw metal oxide ores can be used in some embodiments. Reference is made to Figure 6B, when metal oxide ores are introduced at the top of the fluidized bed the ores, under the influence of the gaseous hydrogen rich environment, are reduced to metal, then mixtures of the active metals and / or metal carbides. In so doing, the metal carbides are fragmented both by lattice dimensional changes as well as under the physical forces of attrition from the inert particles in the fluid bed (e.g., FeOx ^ Fe ^ Fe3C) ). As the macroscopic and dense oxides are reduced, the ore moves down into the bed into more carbon-rich environments which further forms and fragments the materials into the active nanoparticle catalysts from which the low density carbon grows. Figure 6C shows the x-ray diffraction spectra and TEM micrographs of carbon made from catalysts which are predominately iron carbide and iron which were derived from iron oxide, left, and from iron, right, catalyst precursors. Both samples show that highly crystalline graphitic carbon (26 degree peak) is produced from either catalyst precursor source, with the broader iron peak at 45 degreesfor the iron ore (oxide) suggesting smaller iron particles. Evidence of both iron and iron carbide are observed.

[0065] Another feature of the systems and methods disclosed herein allows secondary use of the catalyst when certain mineral ores are fed as catalyst precursors. In several common low cost iron containing ores, there exists substantial amounts of nickel (e.g. laterite ore). In an embodiment, ores containing both iron and nickel can be used as the catalyst precursors. Within the inert containing fluidized bed reactor, the iron and nickel both are reduced and fragmented into the active catalysts on which carbon grows. Upon removal of the iron and nickel containing carbon, the solid product can subsequently be processed by such methods as ball milling or other methods known to the field to disengage substantial fractions of the carbon from the metals. The metals can be separated by density and / or magnetic separation and sold as a separate product for use in metallurgy. Other commonly used methods of separation may also be used to enable the recovery of the metals.

[0066] In some embodiments, additional forms of heat integration can be used with any of the embodiments disclosed herein. As shown in Figure 7, 1 a heat exchange surfaces 70 such as heating tubular coils of any number of thermally conducting materials can be interspersed within the inert particulates at the bottom of the reactor where low temperature feed 10 can enter the fluidized bed. The low temperature feed 10 can cool the inert particles at the bed bottom and allow them to transfer heat to cool a liquid or gas heat transfer fluid within the tubes, which is caused by a pump or blower to move to similar heat exchange surfaces 72 in a solid fluidized bed 74 containing the same or different inert particles. The cool fluid from the bottom of the fluidized bed reactor moves to the top of the fluidized bed heat exchanger and moves through heat exchange surfaces 72 to the bottom of the heat exchanger bed where the fluid within the tubes 72 has been heated as it cools the gases exiting the hot reactor. The higher temperature fluid exits the bottom of the heat exchanger bed 74 and is returned to the heat exchange surfaces 70 at the top of the inert particles at the bottom of the fluidized bed reactor.

[0067] Within the system of Figure 7 (and the similar embodiments disclosed herein), when the externally heated inert particles are returned to the primary fluidized bed reactor from the heating section 46, the inert particles may return at a significantly higher temperature than the desired reactor temperature. In the case of pyrolysis where hydrocarbons might be able to react on the inert particles at this temperature, that undesirable reaction is avoided because of the relatively high ratio of hydrogen to hydrocarbon in the upper sections of the bed where the solids are introduced.

[0068] In some aspects, the metal ores used as part of the catalyst (e.g., as part of the catalyst precursors) can be impure, typically with oxides of silicon, aluminum, and magnesium present. As the ores are processed by the combined actions of the reactant and product gases (hydrocarbons, carbon, and hydrogen), carbon oxides will be produced. Under steady state conditions these gases will be in relatively low concentrations and can be removed in the product gas separation units that follow solids removal (e.g. pressure swing absorption, etc). Further, while in the reactor, the action of the carbon oxides will increase the reactivity of methane decomposition thus increasing conversion. In some embodiments, carbon dioxide might be intentionally added to the feed hydrocarbons to promote the reactivity of the hydrocarbons to form carbon and hydrogen within the reactor.

[0069] Another embodiment of the systems and methods disclosed herein allows for internal heating of the reactor and is shown schematically in Figures 8 and 9. Methane or other hydrocarbon gases in a hydrocarbon feed 10 can be preheated and introduced into the bottom of the reactor 24, which can be predominately filled by virtue of their density with the inert particles segregated to the bottom of the reactor 24 where they contact the relatively low temperature hydrocarbon feed. The contact can pre-heat the hydrocarbon(s) as it rises in a relatively small diameter reactor 24, which can allow for high gas velocity and turbulent fluidization to carry the inert particles up with the gas into a wider bed section in an upper section of the reactor 24 filled primarily with catalyst and solid carbon where pyrolysis occurs at a relatively high rate. The reactant gas with product hydrogen continues upward where it can disengage from the solids in thefreeboard region. The iron catalyst exists primarily as iron carbide, Fe3C and iron. The freeboard of the reactor 24 can be designed such that as the low-density carbon containing trace amounts of iron accumulates in zones separated spatially from zones containing inert particles where the heat transfer surfaces are placed, a fraction of the solid exits the reactor 24 with the hydrogen, and the solids can be separated from the hydrogen using one or more separators 50 such as cyclones and / or filters. The outer regions of the wider section of the fluid bed reactor can have a relatively high mass fraction of the higher density inert particles and heating coils can be positioned within the portion of the bed having a higher inert particle concentration to allow heat to be added to the reactor internally by way of the inert particles.

[0070] In a similar manner as discussed above and as shown in Figure 10, heat integration allowing the hot product gas heat to be exchanged with the entering, relatively cool hydrocarbon feed, can be accomplished by immersion of heat transfer surfaces within the inert bed at the bottom of the reactor with exchange of heat by way of heat transfer fluid and heat exchange surfaces at the reactor exit.

[0071] In the embodiments shown in Figures 8-10, a makeup catalyst stream can be added into the reactor at a variety of locations. In some aspects, the makeup catalyst can be added into the freeboard space and / or the portion of the bed having a higher fraction of solid carbon and catalyst particles (e.g., an upper portion of the particle bed). As described herein, the catalyst particles may initially have a larger size and higher density upon entering the reactor. As the catalyst forms a carbide due to contact with the hydrocarbon under reducing conditions, the catalyst particles may disintegrate to form smaller, nanosized particles that can form solid carbon. The resulting nanoscale catalyst particles with carbon can then rise within the bed due to the density differences within the fluidized bed. The formation of nanoscale catalyst particles and the resulting stratification of the particle bed can occur regardless of where the initial catalyst particles are introduced into the reactor, and as a result, any suitable location to introduce the initial catalyst particles can be used.

[0072] The fluidized bed reactors used for the present invention comprises typically a cylindrical vessel made of a suitable material, such as stainless steel, carbon steel, or other materials known in the art. The vessel can be of a cold wall design and provided with a refractory ceramic lining to minimize heat loss while maintaining the desired reaction temperature. The cold wall design can generally rely on internal linings to maintain heat within the vessel, and the external metal can be open to the atmosphere. This design can allow the outer metal pressure vessel structure to be maintained at a lower temperature, and thereby maintain structural integrity with a simplified design and capital costs.

[0073] The vessel will typically be of smaller diameter at the bottom and increased diameter at the top (e.g., freeboard) with a length-to-diameter ratio of from approximately 3:1 to 10:1, preferably about 5:1 to about 8:1. The vessel can be equipped with an inlet for introducing the reactant gas, and / or other suitable gases known in the art. The gas can be introduced into the vessel through the distributor plate, or manifold which is located at the bottom of the vessel. A distributor plate comprises a plurality of orifices arranged in a circular or concentric circular pattern, which allows the gas to enter the vessel and fluidize the bed of solid particles.

[0074] The reactor further comprises a bed of solid particles which are a novel mixture of a catalytic material, an inert solid, and carbon that are supported by the distributor plate. The size and shape of the particles may vary, but typically range from about 50 to approximately 500 microns in diameter, with the catalyst particles once being reduced, having a size on the nanometer scale.

[0075] The reactor may also be equipped with one or more additional inlets for introducing reactants or solids, into the vessel. The reaction occurs within the bed region containing the catalyst. During operation, the reactant gas (e.g., a hydrocarbon gas) can be introduced into the vessel through the distributor plate, which fluidizes the bed of solid particles. In some embodiments the lowest sections of the bed which is predominately inert particles can be heated by heat exchange with the hot product gas leaving the bed. Although there may be some carbon forming reactions between the heated inert particles and reactant gases, no carbon accumulation will occur because the fluidized inert particleswill physically remove any deposited carbon (attrition). The fluidized bed provides high surface area and good mixing, which enhances the mass transfer and heat transfer rates. The product hydrogen and solid carbon products with a fraction of iron are removed from the vessel through the outlet, which is located at the top of the vessel.

[0076] Another important attribute of the systems and methods disclosed herein is the insensitivity of the continuous process to common hydrocarbon feedstock impurities or contaminants. Sulfur must be removed from most all hydrogen producing processes which have traditional catalysts, and such removal is costly. In some embodiments utilizing iron as the catalyst at temperatures between 800 °C and 1000 °C, sulfur compounds within the feed stream will react and form solid iron sulfide which can be safely removed with the solid carbon product and stored or disposed of. There is no requirement to remove such contaminants although the option to remove the solid products remains available. Further, in natural gas other common contaminants include nitrogen, carbon oxides, and higher hydrocarbons. None of these common contaminants will result in significant impacts on the products or process and do not need to be removed in the continuous process.

[0077] Another important attribute of the systems and methods disclosed herein is the ability to use transition metal oxide ores as precursors for the pyrolysis catalysts. After addition of the ores and subsequent fractionation to form nanoparticulate pyrolysis catalysts, pyrolysis occurs to high carbon-to-metal ratios and the carbon and small fractions of catalyst are removed from the reactor. In embodiments using iron, nickel, manganese, and cobalt, relatively low value oxide ores may be provided to the fluidized bed reactor, and within the pyrolysis environment, the oxide ores are reduced and fragmented into nanoparticulate catalysts comprised of metallic and / or metal carbide character. These catalysts convert the hydrocarbons to hydrogen and solid carbon on which the catalysts remain partially adherent. The carbon co-product removed from the reactor together with the adherent metal / metal carbide catalyst can, if desired, be separated into carbon and metal / metal carbide co-products. The reduced metal / metal carbide co-products are of significantly greater value than the ores fed to the reactor thusincreasing the commercial value of the products. At most reaction temperatures the oxygen in the ores will appear as a CO product. (1+ax)CH4 + aMOx ^ 2(1+ax)H2 + (1-a / n)C + axCO + (a / n)MnC If a zero-CO2 process is desired the product stream can be cooled and the hydrogen caused to react2(1+ax)H2 + (1-a / n)C + axCO + (a / n)MnC ^ 2H2 + axH2O +(1-a / n+ax)C + aMnC In some embodiments, iron ore consisting, for example of Fe2O4, has an overall reaction in the CO2-free cycle of, (1+2a)CH4+ aFeO2^ 2H2+ 2aH2O +(1-a / 3+2a)C + aFe3C In some aspects, a < 0.1 (high yields of carbon and hydrogen per unit mass of iron), nevertheless, when particular value is ascribed to the metal / metal carbide it may be desirable to allow for greater values of a.

[0078] Another feature of the density stratified fluidized bed reactor is illustrated in Figure 11. When a variable diameter fluid bed configuration is employed whereby the diameter increases in the top section and freeboard, the denser inert components of the bed segregate to a relatively narrow section of the reactor where the feed gas is introduced. The void fraction of the high-density region is relatively low (e.g. 0.3-0.6) and the gas residence time in the region is relatively short. The lower density carbon and nanoparticulate solids can be stratified towards the top and have a relatively low void fraction (0.6-0.9), and in this volume where significant catalyst is present, the gas residence time is relatively long allowing for high gas conversion. The lower density product solids can be removed by fluidizing low density solids (high Carbon to catalyst ratio) out from the top of the bed with the outlet product gas, or by a product outlet tube near the top of the bed where solids with minimal product gas are selectively removed. EXAMPLES

[0079] The disclosure having been generally described, the following examples are given as particular embodiments of the disclosure and to demonstrate the practice andadvantages thereof. It is understood that the examples are given by way of illustration and are not intended to limit the specification or the claims in any manner. EXAMPLE 1 Carbon and sand stratification in the fluidized bed reactor

[0080] In a specific example, methane was decomposed into hydrogen and solid carbon in a mixture of sand and iron (20 wt.% Fe). The methane was reacted with iron present in the mixture in a fluidized bed reactor having void fraction of 50 %. The reactor was a quartz tube with 60 cm in length and 1.5 cm inside diameter heated at 950 ℃ and 2 sec residence time. The carbon was grown over iron in the form of Fe3C and graphitic carbon. The product gases were monitored by mass spectrometry and conversion was measured through gas chromatography. The conversion increased initial and attains steady state in approximately 1.5 hr and remained stable more than 8.5 hr at 950 ℃ and 2 sec residence time. Figure 12 shows a schematic representation of the carbon and sand stratified in the bed. Initially iron was added in sand and mixed well to make a uniform distribution of iron in sand. As fluidization started, the bed formed two zone namely, sand rich zone on top and iron rich zone at bottom of reactor due to the difference in their densities. As methane interacted with iron at elevated temperature, carbon started to deposited over iron particles. Over period of time, owing to the graphite precipitation and metal dusting, the particle size of the carbon deposited iron particle changed which resulted into change in their density. Hence, again two zones were formed but now the sand rich zone was on the bottom and the iron and carbon rich zone was on the top of the reactor due to change in their density. There was no deposition on the wall of the reactor. Being an inert material, carbon was not able to deposit over sand. Therefore, carbon deposited over iron was separated through magnetic separation with 99.98% efficiency. The amount of deposited carbon was calculated by weight gain in iron. After 8.5 h of reaction, the C / Fe ratio was above 12.5. The carbon grown over iron exhibited void fraction of 82% after 8.5 h reaction.EXAMPLE 2 The time on stream stability of the catalyst

[0081] In another specific example, methane was pyrolyzed with a mixture of sand and iron (20 wt.% Fe). The methane was converted into solid carbon in a fluidized bed reactor having a void fraction of 50 %. The reactor was a quartz tube with 60 cm in length and 1.5 cm inside diameter heated at 950 ℃ and 2 sec residence time. The carbon was deposited over iron in the form of Fe3C and graphitic carbon. The product gases were monitored by mass spectrometry and conversion was measured through gas chromatography. Figure 13 shows the methane conversion with time on stream. The conversion increases initially and attains a steady state after approximately 1.5 hr and remains stable more than 8.5 hr at 950 ℃ and 2 sec residence time. There was no carbon deposition on the wall of the reactor. Being an inert material, carbon was not able to deposit over sand or the reactor wall. Carbon deposited and grown on the iron catalyst was separated through magnetic separation with 99.98% efficiency. The amount of deposited carbon was calculated by weight gain in iron. After 8.5h reaction, the C / Fe ratio was above 12.5. EXAMPLE 3 The effect of gas residence time

[0082] In another specific example, methane decomposition was carried out in a mixture of sand and iron (20 wt.% Fe). The methane was converted into solid carbon in a fluidized bed reactor with a void fraction of 50 %. The reactor was a quartz tube with 60 cm in length and 1.5 cm inside diameter heated at 950 ℃ and varying residence time from 1.3 sec to 3.3 sec. The carbon was deposited over iron in the form of Fe3C and graphitic carbon. The product gases were monitored by mass spectrometry and conversion was measured through gas chromatography. Figure 14 shows the effect of residence time on methane conversion. The conversion increases with an increase in residence time from 1.3 sec to 3.3 sec at 950 ℃. The reactor was operated from 2-2.5 hrto reach the steady state at 950 ℃ and 2 sec residence time. After that, the flow was adjusted to the desired residence time and maintained for at least 0.5-1 hr. EXAMPLE 4 The effect of temperature with varying composition of iron at low and high residence times

[0083] In another specific example, methane was reacted with iron in a mixture of sand and iron. The methane was converted into solid carbon in a fluidized bed reactor void fraction of 40 to 50 % depending upon the ratio of iron and sand. To be very specific, the void fraction of pure sand and 20% iron in sand was 40% and 50% respectively. The ratio of iron in sand was varied from pure sand to 70% sand with 30% iron. The reactor was a quartz tube with 60 cm in length and 1.5 cm inside diameter heated in the temperature range of 650-950 ℃ with a flow of 243 ml / min at 1.3 sec residence time. The carbon was deposited over iron in the form of Fe3C and graphitic carbon. The product gases were monitored by mass spectrometry and conversion was measured through gas chromatography. Figure 15 shows the effect of temperature on methane conversion with varied composition of iron also. The conversion increases with an increase in temperature from 650℃ to 950 ℃ and also with increasing the iron loading in sand. The reactor was operated over 2-2.5 hr to reach the steady state at 950 ℃ and 1.3 sec residence time. After that, the temperature was varied to the desired reaction temperatures and kept at least 0.5- 1 hr.

[0084] In a separate experiment with a longer residence time, methane was reacted in a mixture of sand and iron. The methane was decomposed into solid carbon in a fluidized bed reactor void fraction of 40 to 50 % depending upon the ratio of iron and sand. The void fraction of pure sand and 20% iron in sand was 40% and 50% respectively. The ratio of iron in sand was varied from pure sand to 70% sand with 30% iron. The reactor was a quartz tube with 60 cm in length and 1.5 cm inside diameter heated in the temperature range of 650-950 ℃ with a flow of 105 ml / min at 2 sec residence time. The carbon was deposited over iron in the form of Fe3C and graphitic carbon. The product gases weremonitored by mass spectrometry and conversion was measured through gas chromatography. Figure 15 shows the effect of iron loading on methane conversion with time on stream. The conversion increases initial and attains steady state in approximately 1.5 hr and remains stable at 950 ℃ and 2 sec residence time. EXAMPLE 5 The effect of temperature with varying composition of iron at high residence time

[0085] In another specific example, methane was reacted with iron in a mixture of sand and iron. The methane was converted into solid carbon in a fluidized bed reactor void fraction of 40 to 50 % depending upon the ratio of iron and sand. To be very specific, the void fraction of pure sand and 20% iron in sand was 40% and 50% respectively. The ratio of iron in sand was varied from pure sand to 70% sand with 30% iron. The reactor is a quartz tube with 60 cm in length and 1.5 cm inside diameter heated in the temperature range of 650-950 ℃ with a flow of 105 ml / min at 2 sec residence time. The carbon was deposited over iron in the form of Fe3C and graphitic carbon. The product gases were monitored by mass spectrometry and conversion was measured through gas chromatography. Figure 16 shows the effect of temperature on methane conversion with varied composition of iron. The conversion increases with an increase in temperature from 650℃ to 950 ℃ and also with increasing the iron loading in the sand. The reactor was operated from 2-2.5 hr to reach the steady state at 950 ℃ and 2 sec residence time. After that, the temperature was switched to desired reaction temperatures and kept at least 0.5-1 hr. EXAMPLE 6 Pyrolysis of crude natural with sulfur contaminants in iron / inert fluidized bed reactor

[0086] In a prophetic example, raw natural gas containing primarily methane with common additional components including ethane, propane, CO2, nitrogen, and sulfur containing compounds is fed to the fluid bed reactor containing 80 weight percent sand and 20 weight percent iron at 950 C. The total flowrate is 300 sccm. The gas phaseproducts are analyzed by gas chromatography and found to contain only hydrogen and methane. The methane conversion is 87% while complete conversion of other hydrocarbons is observed. No sulfur containing gas-phase products are observed. The overall methane conversion is 91% at 1 atm pressure. Analysis of the solids after the reaction shows the presence of solid iron sulfide. EXAMPLE 7 Pyrolysis of methane in the in iron / inert or iron oxide / inert tapered fluidized bed reactor

[0087] In a specific example, methane was pyrolysed into hydrogen and solid carbon in a mixture of sand and iron (20wt.% Fe) and iron oxide (20 wt.% Fe). The methane was reacted with iron present in a mixture in a fluidized bed reactor void fraction of 50 %. The reactor was a tapered quartz tube with 75 cm in length and 1 cm inside diameter at bottom till 20 cm height and then diameter gradually increased to 25 cm and heated at 950 ℃ and 1.2 sec residence time. The carbon was deposited over iron and iron oxide in the form of Fe3C and graphitic carbon. The product gases were monitored by mass spectrometry and conversion was measured through gas chromatography. The conversion increases initial and attained steady state in approximately 1.5 hr and remained stable more than 8.5 hr at 950 ℃ and 1.2 sec residence time. Figure 17 shows the methane conversion with time on stream on both iron and iron oxide. The conversion increased initial and attained steady state in approximately 1.5 hr and remained stable more than 12 hr at 950 ℃ and 1.2 sec residence time. There was no deposition on the wall of the reactor. Being an inert material, carbon was not able to deposit over sand. Therefore, the carbon that deposited and grew over iron was separated through magnetic separation with 99.98% efficiency. The amount of deposited carbon was calculated by weight gain in iron. After reaction, the atomic C / Fe ratio in both iron oxide and iron were 23 and 30 (4.92 and 6.6 by weight) respectively.EXAMPLE 8 Methane decomposition in the in iron / inert or iron oxide / inert tapered fluidized bed reactor

[0088] In another example, methane was decomposed into hydrogen and solid carbon in a mixture of sand and iron (20wt.% Fe) and iron oxide (20 wt.% Fe). The methane was reacted with iron present in mixture in a fluidized bed reactor void fraction of 50 %. The reactor was a tapered quartz tube with 75 cm in length and 1 cm inside diameter at bottom till 20 cm height and then diameter gradually increased to 25 cm and heated at 950 ℃ and 1.2 sec residence time. The carbon was deposited over iron and iron oxide in the form of Fe3C and graphitic carbon. The product gases were monitored by mass spectrometry and conversion was measured through gas chromatography. The conversion increased initial and attained steady state in approximately 1.5 hr and remained stable more than 8.5 hr at 950 ℃ and 1.2 sec residence time. Figure 18 shows XRD profile of iron and oxide after 12 h reaction. Peak appeared at 2 ^^ ൌ ~26 degrees is corresponded to graphitic carbon. The same peak also appears in Fe3C but their peak intensity is very low. Peak positioned at ~45 degree could be attributed to the presence of graphitic carbon / iron or Fe3C also. The intensity of the peak position at ~45 degree is higher in the case of iron oxide than iron which is attributed to the high amount to C / Fe ratio. The atomic C / Fe ratio in both iron oxide and iron were 23 and 30 (4.92 and 6.6 by weight) respectively. Similarly, as C / Fe ratio is increasing over time the intensity of the peak position at ~45 degree is also decreasing which confirm the increasing C / Fe ratio over time. EXAMPLE 9 XRD profile of the carbon deposited over sand without iron at 1200℃

[0089] In a specific example, methane was pyrolysed into hydrogen and solid carbon in a sand bed fluidized bed reactor void fraction of 42 %. The reactor was a quartz tube with 70 cm in length and 0.7 cm inside diameter heated at 1000-1200 ℃ and 2 sec residence time. The carbon was deposited over sand and wall of the reactor. The product gases were monitored by mass spectrometry and conversion was measured through gaschromatography. The conversion increased rapidly and attained steady state within few seconds and remains stable more than 3 hr at 1200 ℃ and 2 sec residence time. Figure 19 shows XRD profile of carbon deposited over sand without iron after 3 h reaction at 1200℃ and 2 sec residence time. The very high intensity peaks appeared at 2 ^^ ൌ ~20.95, 26.7 and 50.27 degrees are attributed to presence of SiO2as present in quartz which matches well with PDF No. (03-065-0466). The corresponding peaks for graphitic carbon was missing in carbon deposited over sand. Only broad hump appeared near 26 degree which confirm the presence of amorphous carbon which is in agreement with the results obtained through RAMAN characterization as shown in Figure 1. The intensity of the peak positioned at 2 ^^ ൌ ~20.95 is relatively high in the case of carbon deposited over sand which suggest the presence of only sand particles rather than carbon. The intensity of the peak appeared at 2 ^^ ൌ ~20.95 and 50.27 should have decreased if graphitic carbon is deposited over sand particles which further indicates the presence of only amorphous carbon over sand particles.   ALTERNATIVES

[0090] Having described various systems, methods, and compositions, certain aspects can include, but are not limited to:

[0091] In a first aspect, a system for converting hydrocarbons gases to solid carbon and hydrogen products comprises: a pyrolysis reactor 22 comprising a bed of particulates, wherein the bed of particulates comprises catalyst particles, solid carbon, and inert particles, wherein the pyrolysis reactor 22 comprises a feed gas 10 inlet at a lower portion of the bed of particulates, a product gas and solid outlet 44 above the bed of particulates; and a separator 42 in fluid communication with the pyrolysis reactor 22 through the product gas outlet, where the separator 42 is configured to separate any particulates in a product gas produced in the pyrolysis reactor 22.

[0092] A second aspect can include the system of the first aspect, wherein the particulates within the bed of particulate are configured to be fluidized by gases traveling from the bottom of the reactor 22 to the outlet such that relatively dense heated inert particlesintroduced at the top of the reactor will intermix with the solid carbon and catalyst within the reactor and migrate to the bottom of the reactor 22 allowing for their selective withdrawal at the bottom of the reactor.

[0093] A third aspect can include the system of the first or second aspect, wherein the pyrolysis reactor 22 further comprises: a particulate outlet above the feed gas inlet configured to selectively remove the inert particles from the bed of particulates; a particulate inlet near the top of the bed of particulates configured to provide heated inert particles to the reactor; and a solids heating section 46 in fluid communication with the particulate outlet and the particulate inlet, wherein the solids heating section is configured to accept a portion of the inert particulates from the pyrolysis reactor through the particulate outlet, heat the portion of the inert particulates to form heated particulates, and return the heated particulates to the pyrolysis reactor through the particulate inlet.

[0094] A fourth aspect can include the system of the third aspect, further comprising: a non-mechanical valve coupled between the particulate outlet and the solids heating section, and between the heated particulate separator returning solids to the reactor inlet.

[0095] A fifth aspect can include the system of the third or fourth aspect, wherein the solids heating section 46 comprises: a riser configuration to receive a portion of the particulates from the bed of particulates; and at least one of: i) an inlet to accept a high temperature gas heated prior to contacting the particulates by combustion or electric heating, or ii) an oxygen containing gas inlet and combustion gas inlet configured to combust a combustion gas within the riser, wherein the solids heating section is configured to contact the portion of the particulates with the combustion gas and the oxygen containing gas, combust the combustion gas, and heat the portion of the particulates.

[0096] A sixth aspect can include the system of the fifth aspect, wherein the solids heating section 46 further comprises: a second separator 48 configured to receive the portion of the particulates downstream of the riser, wherein the second separator 48 is configured to separate and return the particulates to the pyrolysis reactor.

[0097] A seventh aspect can include the system of any one of the first to sixth aspects, further comprising: one or more secondary separators, wherein the one or more secondary separators are configured to receive an outlet product gas from the separator and separate any particulates in the outlet product gas.

[0098] An eighth aspect can include the system of any one of the third to seventh aspects, wherein one or more of the, pyrolysis reactor 22, the solids heating section 46, the solid transfer lines, or the separator 42 have a cold wall design.

[0099] A ninth aspect can include the system of any one of the first to eighth aspects, wherein the catalyst is configured to be added to the pyrolysis reactor 22 in one form and is transformed within the reactor to the active catalyst.

[0100] A tenth aspect can include the system of any one of the first to eighth aspects, wherein the catalyst particles comprise iron ore, pig iron, iron, iron oxide, and wherein the catalyst particles are configured to form a catalytic material within the pyrolysis reactor when contacted by the hydrocarbon reactant.

[0101] An eleventh aspect can include the system of any one of the first to eighth aspects, wherein the inert material comprises sand, gravel, magnesia, alumina, zirconia, or any combination thereof.

[0102] A twelfth aspect can include the system of any one of the first to eleventh aspects, wherein the catalyst particles comprise iron, nickel, cobalt, manganese, or any combination thereof.

[0103] A thirteenth aspect can include the system of any one of the first to twelfth aspects, wherein the catalyst particles have a diameter on a nanometer scale.

[0104] A fourteenth aspect can include the system of any one of the first to thirteenth aspects, wherein the inert particles have a diameter between 0.01 – 10 mm.

[0105] A fifteenth aspect can include the system of any one of the first to fourteenth aspects, wherein the catalyst particles make up between about 1 – 70 wt.% of the bed of particulates.

[0106] A sixteenth aspect can include the system of any one of the first to fifteenth aspects, wherein the bed of particulates comprises a stratified bed of particulates,wherein a majority of the inert particles are in a lower portion of the bed, and wherein the solid carbon and catalyst particles are in an upper portion of the bed.

[0107] In a seventeenth aspect, a fluidized bed reaction process comprises: contacting a hydrocarbon reactant with a fluidized bed within a reactor, wherein the fluidized bed comprises catalyst particles, solid carbon, and inert particles; stratifying the fluidized bed within the reactor, wherein the inert particles move to a lower portion of the fluidized bed, and wherein the solid carbon and catalyst particles move to an upper portion of the fluidized bed; forming the solid carbon and hydrogen based on contacting the hydrocarbon reactant with the fluidized bed; and removing the hydrogen and at least a portion of the solid carbon from the reactor.

[0108] An eighteenth aspect can include the process of the seventeenth aspect, further comprising: removing at least a portion of the inert particles from the lower portion of the fluidized bed; heating the portion of the inert particles to form heated inert particles; and passing the heated inert particles to the upper portion of the fluidized bed.

[0109] A nineteenth aspect can include the process of the eighteenth aspect, wherein the portion of inert particles removed from the lower portion of the fluidized bed is substantially free of solid carbon or catalyst particles.

[0110] A twentieth aspect can include the process of the eighteenth aspect, wherein heating the portion of the inert particles comprises: using solar heating to heat the inert particles.

[0111] A twenty first aspect can include the process of the eighteenth aspect, wherein heating the portion of the inert particles comprises:

[0112] combusting a combustion gas and contacting the combustion gas with the portion of the inert particles

[0113] A twenty second aspect can include the process of the eighteenth aspect, wherein heating the portion of the inert particles comprises: using electrical heating.

[0114] A twenty third aspect can include the process of any one of the eighteenth to twenty second aspects, further comprising: heating the catalyst particles in the upperportion of the fluidized bed with the heated inert particles; and passing the heated inert particles from the upper portion to the lower portion of the fluidized bed.

[0115] A twenty fourth aspect can include the process of any one of the seventeenth to twenty third aspects, further comprising: forming the solid carbon on the catalyst particles; and

[0116] removing a portion of the solid carbon from the catalyst particles using the inert particles.

[0117] A twenty fifth aspect can include the process of any one of the seventeenth to twenty fourth aspects, further comprising: removing a portion of the catalyst particles from the reactor with the solid carbon; and separating the portion of the catalyst particles from the solid carbon in a separator.

[0118] A twenty sixth aspect can include the process of the twenty fifth aspect, wherein the separator comprises a cyclone separator or a magnetic separator.

[0119] A twenty seventh aspect can include the process of any one of the seventeenth to twenty sixth aspects, further comprising: introducing catalyst precursor particles into the reactor; and converting the catalyst precursor particles into the catalyst particles within the reactor based on contacting the hydrocarbon with the catalyst precursor particles.

[0120] A twenty eighth aspect can include the process of any one of the seventeenth to twenty seventh aspects, wherein the contacting occurs at a temperature below a reaction temperature of the hydrocarbon reactant with the inert particles and above a reaction temperature of the hydrocarbon reactant and the catalyst particles.

[0121] A twenty ninth aspect can include the process of any one of the seventeenth to twenty eighth aspects, wherein the reactor comprises a tapered bed having an upper portion with a diameter greater than a diameter of the lower portion.

[0122] A thirtieth aspect can include the process of any one of the seventeenth to twenty ninth aspects, wherein contacting the hydrocarbon reactant with the fluidized bed within the reactor occurs at a temperature between 600-1000 °C.

[0123] A thirty first aspect can include the process of any one of the seventeenth to thirtieth aspects, wherein the solid carbon is graphitic carbon.

[0124] A thirty second aspect can include the process of any one of the seventeenth to thirty first aspects, wherein the catalyst particles comprise iron, nickel, manganese, cobalt, oxides thereof, ores thereof, and / or combinations thereof.

[0125] A thirty third aspect can include the process of any one of the seventeenth to thirty second aspects, wherein the catalyst particles have a size from 1 to 1,000 nanometers.

[0126] A thirty fourth aspect can include the process of any one of the seventeenth to thirty third aspects, further comprising: introducing one or more catalyst promotors into the reactor, wherein the one or more catalyst promotors comprise an alkali metal nitrate, an alkali halide salt, a hydrogen halide, an alkylhalide, a halogen, or a combination thereof.

[0127] A thirty fifth aspect can include the process of any one of the seventeenth to thirty fourth aspects, wherein the inert particles comprise sand, gravel, magnesia, alumina, zirconia, or any combination thereof.

[0128] A thirty sixth aspect can include the process of any one of the seventeenth to thirty fifth aspects, wherein the inert particles have a size in a range of between about 0.01 to about 10 mm

[0129] A thirty seventh aspect can include the process of any one of the seventeenth to thirty sixth aspects, wherein the catalyst particles comprise 1-70 wt.% of the particle bed.

[0130] A thirty eighth aspect can include the process of any one of the seventeenth to thirty seventh aspects, wherein the hydrocarbon reactant is contacted with the fluidized bed for a time between 0.1 to 10 seconds.

[0131] A thirty ninth aspect can include the process of any one of the seventeenth to thirty eighth aspects, wherein the solid carbon is produced at a weight ratio of the solid carbon to the catalyst particles of greater than 7.

[0132] A fortieth aspect can include the process of any one of the seventeenth to thirty ninth aspects, further comprising: exchanging heat between the hydrocarbon and carbon in the upper portion and the hydrocarbon reactants in the lower portion.

[0133] A forty first aspect can include the process of any one of the seventeenth to fortieth aspects, further comprising: contacting the outlet gas with a second particle bed; and exchanging heat with the second particle bed and the inert particles in the lower portion of the reactor.

[0134] A forty second aspect can include the process of any one of the seventeenth to forty first aspects, wherein the hydrocarbon reactant comprises methane, ethane, natural gas, alkenes, alcohols, pyrolyzed products of a hydrocarbon liquid, or solid hydrocarbons.

[0135] A forty third aspect can include the process of any one of the seventeenth to forty second aspects, wherein the reactor has a cold wall design.

[0136] In a forty fourth aspect, a fluidized bed reaction process comprises: contacting a hydrocarbon reactant with a fluidized bed within a reactor, wherein the fluidized bed comprises catalyst particles, solid carbon, and inert particles, wherein the hydrocarbon reactant comprises an impurity; stratifying the fluidized bed within the reactor, wherein the inert particles move to a lower portion of the fluidized bed, and wherein the solid carbon and catalyst particles move to an upper portion of the fluidized bed; forming the solid carbon and hydrogen based on contacting the hydrocarbon reactant with the fluidized bed; reacting at least a portion of the impurity with a portion of the catalyst particles; and removing the hydrogen and at least a portion of the solid carbon from the reactor.

[0137] A forty fifth aspect can include the process of the forty fourth aspect, further comprising: removing at least a portion of the inert particles from the lower portion of the fluidized bed; combusting at least a portion of the hydrogen to heat the inert particles and form heated inert particles; and passing the heated inert particles to the upper portion of the fluidized bed.

[0138] A forty sixth aspect can include the process of the forty fifth aspect, wherein the portion of inert particles removed from the lower portion of the fluidized bed is substantially free of solid carbon or catalyst particles.

[0139] A forty seventh aspect can include the process of the forty fifth aspect, wherein heating the portion of the inert particles comprises: using solar heating to heat the inert particles.

[0140] A forty eighth aspect can include the process of the forty fifth aspect, wherein heating the portion of the inert particles comprises: combusting a combustion gas and contacting the combustion gas with the portion of the inert particles

[0141] A forty ninth aspect can include the process of the forty fifth aspect, wherein heating the portion of the inert particles comprises: using electrical heating.

[0142] A fiftieth aspect can include the process of any one of the forty fifth to forty ninth aspects, further comprising: heating the catalyst particles in the upper portion of the fluidized bed with the heated inert particles; and passing the heated inert particles from the upper portion to the lower portion of the fluidized bed.

[0143] A fifty first aspect can include the process of any one of the forty fourth to fiftieth aspects, further comprising: forming the solid carbon on the catalyst particles; and removing a portion of the solid carbon from the catalyst particles using the inert particles.

[0144] A fifty second aspect can include the process of any one of the forty fourth to fifty first aspects, further comprising: removing a portion of the catalyst particles from the reactor with the solid carbon; and separating the portion of the catalyst particles from the solid carbon in a separator.

[0145] A fifty third aspect can include the process of the fifty second aspect, wherein the separator comprises a cyclone separator or a magnetic separator.

[0146] A fifty fourth aspect can include the process of any one of the forty fourth to fifty third aspects, further comprising: introducing catalyst precursor particles into the reactor; and converting the catalyst precursor particles into the catalyst particles within the reactor based on contacting the hydrocarbon with the catalyst precursor particles.

[0147] A fifty fifth aspect can include the process of any one of the forty fourth to fifty fourth aspects, wherein the contacting occurs at a temperature below a reaction temperature of the hydrocarbon reactant with the inert particles and above a reaction temperature of the hydrocarbon reactant and the catalyst particles.

[0148] A fifty sixth aspect can include the process of any one of the forty fourth to fifty fifth aspects, wherein the reactor comprises a tapered bed having an upper portion with a diameter greater than a diameter of the lower portion.

[0149] A fifty seventh aspect can include the process of any one of the forty fourth to fifty sixth aspects, wherein contacting the hydrocarbon reactant with the fluidized bed within the reactor occurs at a temperature between 600-1000 °C.

[0150] A fifty eighth aspect can include the process of any one of the forty fourth to fifty seventh aspects, wherein the solid carbon is graphitic carbon.

[0151] A fifty ninth aspect can include the process of any one of the forty fourth to fifty eighth aspects, wherein the catalyst particles comprise iron, nickel, manganese, cobalt, oxides thereof, ores thereof, and / or combinations thereof.

[0152] A sixtieth aspect can include the process of any one of the forty fourth to fifty ninth aspects, wherein the catalyst particles have a size from 1 to 1,000 nanometers.

[0153] A sixty first aspect can include the process of any one of the forty fourth to sixtieth aspects, further comprising: introducing one or more catalyst promotors into the reactor, wherein the one or more catalyst promotors comprise an alkali metal nitrate, an alkali halide salt, a hydrogen halide, an alkylhalide, a halogen, or a combination thereof.

[0154] A sixty second aspect can include the process of any one of the forty fourth to sixty first aspects, wherein the inert particles comprise sand, gravel, magnesia, alumina, zirconia, or any combination thereof.

[0155] A sixty third aspect can include the process of any one of the forty fourth to sixty second aspects, wherein the inert particles have a size in a range of between about 0.01 to about 10 mm

[0156] A sixty fourth aspect can include the process of any one of the forty fourth to sixty third aspects, wherein the catalyst particles comprise 1-70 wt.% of the particle bed.

[0157] A sixty fifth aspect can include the process of any one of the forty fourth to sixty fourth aspects, wherein the hydrocarbon reactant is contacted with the fluidized bed for a time between 0.1 to 10 seconds.

[0158] A sixty sixth aspect can include the process of any one of the forty fourth to sixty fifth aspects, wherein the solid carbon is produced at a weight ratio of the solid carbon to the catalyst particles of greater than 7.

[0159] A sixty seventh aspect can include the process of any one of the forty fourth to sixty sixth aspects, further comprising: exchanging heat between the hydrocarbon and carbon in the upper portion and the hydrocarbon reactants in the lower portion.

[0160] A sixty eighth aspect can include the process of any one of the forty fourth to sixty seventh aspects, further comprising: contacting the outlet gas with a second particle bed; and exchanging heat with the second particle bed and the inert particles in the lower portion of the reactor.

[0161] A sixty ninth aspect can include the process of any one of the forty fourth to sixty eighth aspects, wherein the hydrocarbon reactant comprises methane, ethane, natural gas, alkenes, alcohols, pyrolyzed products of a hydrocarbon liquid, or solid hydrocarbons.

[0162] A seventieth aspect can include the process of any one of the forty fourth to sixty ninth aspects, wherein the reactor has a cold wall design. REFERENCES

[0163] The following references, which are identified by [x] in the description above, are incorporated by reference herein:

[0164] [1] H.T. Jang, W.S. Cha, Hydrogen production by the thermocatalytic decomposition of methane in a fluidized bed reactor, Korean Journal of Chemical Engineering.24 (2007) 374–377.

[0165] [2] D. Torres, S. De Llobet, J.L. Pinilla, M.J. Lázaro, I. Suelves, R. Moliner, Hydrogen production by catalytic decomposition of methane using a Fe-based catalyst in a fluidized bed reactor, Journal of Natural Gas Chemistry.21 (2012) 367–373. https: / / doi.org / 10.1016 / S1003-9953(11)60378-2.

[0166] [3] M. Keller, A. Matsumura, A. Sharma, Spray-dried Fe / Al2O3 as a carbon carrier for COx-free hydrogen production via methane cracking in a fluidized bed process, Chemical Engineering Journal. 398 (2020). https: / / doi.org / 10.1016 / j.cej.2020.125612.

[0167] [4] M. Keller, A. Sharma, Hydrogen Production via Methane Cracking on Dry-Coated Fe / ZrO2with Support Recycle in a Fluidized Bed Process, Energy and Fuels.35 (2021) 847–855. https: / / doi.org / 10.1021 / acs.energyfuels.0c03287.

[0168] [5] J.X. Qian, L.R. Enakonda, W.J. Wang, D. Gary, P. Del-Gallo, J.M. Basset, D. Bin Liu, L. Zhou, Optimization of a fluidized bed reactor for methane decomposition over Fe / Al2O3 catalysts: Activity and regeneration studies, Int J Hydrogen Energy. 44 (2019) 31700–31711. https: / / doi.org / 10.1016 / j.ijhydene.2019.10.058.

[0169] [6] L. Zhou, L.R. Enakonda, S. Li, D. Gary, P. Del-Gallo, C. Mennemann, J.M. Basset, Iron ore catalysts for methane decomposition to make COx free hydrogen and carbon nano material, J Taiwan Inst Chem Eng. 87 (2018) 54–63. https: / / doi.org / 10.1016 / j.jtice.2018.03.008.

[0170] [7] J.X. Qian, D. Bin Liu, J.M. Basset, L. Zhou, Methane decomposition to produce hydrogen and carbon nanomaterials over costless, iron- containing catalysts, J Clean Prod. 320 (2021). https: / / doi.org / 10.1016 / j.jclepro.2021.128879.

[0171] [8] R. Siriwardane, J. Riley, C. Atallah, M. Bobek, Investigation of methane and ethane pyrolysis with highly active and durable iron-alumina catalyst toproduce hydrogen and valuable nano carbons: Continuous fluidized bed tests and reaction rate analysis, Int J Hydrogen Energy. (2023). https: / / doi.org / 10.1016 / j.ijhydene.2022.12.268.

[0172] [9] G. Patrianakos, M. Kostoglou, A.G. Konstandopoulos, Effect of seeding on hydrogen and carbon particle production in a 10 MW solar thermal reactor for methane decomposition, in: Int J Hydrogen Energy, 2012: pp. 16570–16580. https: / / doi.org / 10.1016 / j.ijhydene.2012.02.046. CONCLUSION

[0173] Embodiments are discussed herein with reference to the Figures. However, those skilled in the art will readily appreciate that the detailed description given herein with respect to these figures is for explanatory purposes as the systems and methods extend beyond these limited embodiments. For example, it should be appreciated that those skilled in the art will, in light of the teachings of the present description, recognize a multiplicity of alternate and suitable approaches, depending upon the needs of the particular application, to implement the functionality of any given detail described herein, beyond the particular implementation choices in the following embodiments described and shown. That is, there are numerous modifications and variations that are too numerous to be listed but that all fit within the scope of the present description. Also, singular words should be read as plural and vice versa and masculine as feminine and vice versa, where appropriate, and alternative embodiments do not necessarily imply that the two are mutually exclusive.

[0174] It is to be further understood that the present description is not limited to the particular methodology, compounds, materials, manufacturing techniques, uses, and applications, described herein, as these may vary. It is also to be understood that the terminology used herein is used for the purpose of describing particular embodiments only, and is not intended to limit the scope of the present systems and methods. It must be noted that as used herein and in the appended claims (in this application, or any derived applications thereof), the singular forms “a,” “an,” and “the” include the plural referenceunless the context clearly dictates otherwise. Thus, for example, a reference to “an element” is a reference to one or more elements and includes equivalents thereof known to those skilled in the art. All conjunctions used are to be understood in the most inclusive sense possible. Thus, the word “or” should be understood as having the definition of a logical “or” rather than that of a logical “exclusive or” unless the context clearly necessitates otherwise. Structures described herein are to be understood also to refer to functional equivalents of such structures. Language that may be construed to express approximation should be so understood unless the context clearly dictates otherwise.

[0175] Unless defined otherwise, all technical and scientific terms used herein have the same meanings as commonly understood by one of ordinary skill in the art to which this description belongs. Preferred methods, techniques, devices, and materials are described, although any methods, techniques, devices, or materials similar or equivalent to those described herein may be used in the practice or testing of the present systems and methods. Structures described herein are to be understood also to refer to functional equivalents of such structures. The present systems and methods will now be described in detail with reference to embodiments thereof as illustrated in the accompanying drawings.

[0176] From reading the present disclosure, other variations and modifications will be apparent to persons skilled in the art. Such variations and modifications may involve equivalent and other features which are already known in the art, and which may be used instead of or in addition to features already described herein.

[0177] Although claims may be formulated in this application or of any further application derived therefrom, to particular combinations of features, it should be understood that the scope of the disclosure also includes any novel feature or any novel combination of features disclosed herein either explicitly or implicitly or any generalization thereof, whether or not it relates to the same systems or methods as presently claimed in any claim and whether or not it mitigates any or all of the same technical problems as do the present systems and methods.

[0178] Features which are described in the context of separate embodiments may also be provided in combination in a single embodiment. Conversely, various features which are, for brevity, described in the context of a single embodiment, may also be provided separately or in any suitable sub-combination. The Applicant(s) hereby give notice that new claims may be formulated to such features and / or combinations of such features during the prosecution of the present Application or of any further Application derived therefrom.

Claims

CLAIMS 1. A system for converting hydrocarbons gases to solid carbon and hydrogen products, the system comprising: a pyrolysis reactor comprising a bed of particulates, wherein the bed of particulates comprises catalyst particles, solid carbon, and inert particles, wherein the pyrolysis reactor comprises a feed gas inlet at a lower portion of the bed of particulates, a product gas and solid outlet above the bed of particulates; and a separator in fluid communication with the pyrolysis reactor through the product gas outlet, where the separator is configured to separate any particulates in a product gas produced in the pyrolysis reactor.

2. The system of claim 1, wherein the particulates within the bed of particulates are configured to be fluidized by gases traveling from the bottom of the reactor to the outlet such that relatively dense heated inert particles introduced at the top of the reactor will intermix with the solid carbon and catalyst within the reactor and migrate to the bottom of the reactor allowing for their selective withdrawal at the bottom of the reactor.

3. The system of claim 1, wherein the pyrolysis reactor further comprises: a particulate outlet above the feed gas inlet configured to selectively remove the inert particles from the bed of particulates; a particulate inlet near the top of the bed of particulates configured to provide heated inert particles to the reactor; and a solids heating section in fluid communication with the particulate outlet and the particulate inlet, wherein the solids heating section is configured to accept a portion of the inert particulates from the pyrolysis reactor through the particulate outlet, heat the portion of the inert particulates to form heated particulates, and return the heated particulates to the pyrolysis reactor through the particulate inlet.

4. The system of claim 3, further comprising: a first non-mechanical valve coupled between the particulate outlet and the solids heating section; and a second non-mechanical valve coupled between the heated particulate separator returning solids to the reactor inlet.

5. The system of claim 3, wherein the solids heating section comprises: a riser configuration to receive a portion of the particulates from the bed of particulates; and at least one of: i) an inlet to accept a high temperature gas heated prior to contacting the particulates by combustion or electric heating, or ii) an oxygen containing gas inlet and combustion gas inlet configured to combust a combustion gas within the riser, wherein the solids heating section is configured to contact the portion of the particulates with the combustion gas and the oxygen containing gas, combust the combustion gas, and heat the portion of the particulates.

6. The system of claim 5, wherein the solids heating section further comprises: a second separator configured to receive the portion of the particulates downstream of the riser, wherein the second separator is configured to separate and return the particulates to the pyrolysis reactor.

7. The system of claim 1, further comprising: one or more secondary separators, wherein the one or more secondary separators are configured to receive an outlet product gas from the separator and separate any particulates in the outlet product gas.

8. The system of claim 1, wherein one or more of the pyrolysis reactor, the solids heating section, the solid transfer lines, or the separator have a cold wall design.

9. The system of claim 1, wherein the catalyst particles comprise iron ore, pig iron, iron, iron oxide, and wherein the catalyst particles are configured to form a catalytic material within the pyrolysis reactor when contacted by the hydrocarbon reactant.

10. The system of claim 1, wherein the inert material comprises sand, gravel, magnesia, alumina, zirconia, or any combination thereof.

11. The system of claim 1, wherein the catalyst particles comprise iron, nickel, cobalt, manganese, or any combination thereof.

12. The system of claim 1, wherein the catalyst particles have a diameter on a nanometer scale.

13. The system of claim 1, wherein the inert particles have a diameter between 0.01 – 10 mm.

14. The system of claim 1, wherein the catalyst particles make up between about 1 – 70 wt.% of the bed of particulates.

15. The system of claim 1, wherein the bed of particulates comprises a stratified bed of particulates, wherein a majority of the inert particles are in a lower portion of the bed, and wherein the solid carbon and catalyst particles are in an upper portion of the bed.

16. A fluidized bed reaction process comprising: contacting a hydrocarbon reactant with a fluidized bed within a reactor, wherein the fluidized bed comprises catalyst particles, solid carbon, and inert particles; stratifying the fluidized bed within the reactor, wherein the inert particles move to a lower portion of the fluidized bed, and wherein the solid carbon and catalyst particles move to an upper portion of the fluidized bed; forming the solid carbon and hydrogen based on contacting the hydrocarbon reactant with the fluidized bed; and removing the hydrogen and at least a portion of the solid carbon from the reactor.

17. The process of claim 16, further comprising: removing at least a portion of the inert particles from the lower portion of the fluidized bed; heating the portion of the inert particles to form heated inert particles; andpassing the heated inert particles to the upper portion of the fluidized bed.

18. The process of claim 17, wherein heating the portion of the inert particles comprises: using solar heating to heat the inert particles, combusting a combustion gas and contacting the combustion gas with the portion of the inert particles, or using electrical heating.

19. The process of claim 17, further comprising: heating the catalyst particles in the upper portion of the fluidized bed with the heated inert particles; and passing the heated inert particles from the upper portion to the lower portion of the fluidized bed.

20. The process of claim 16, further comprising: forming the solid carbon on the catalyst particles; and removing a portion of the solid carbon from the catalyst particles using the inert particles.

21. The process of claim 16, further comprising: removing a portion of the catalyst particles from the reactor with the solid carbon; and separating the portion of the catalyst particles from the solid carbon in a separator.

22. The process of claim 21, wherein the separator comprises a cyclone separator or a magnetic separator.

23. The process of claim 16, further comprising: introducing catalyst precursor particles into the reactor; and converting the catalyst precursor particles into the catalyst particles within the reactor based on contacting the hydrocarbon with the catalyst precursor particles.

24. The process of claim 16, wherein the contacting occurs at a temperature below a reaction temperature of the hydrocarbon reactant with the inert particles andabove a reaction temperature of the hydrocarbon reactant and the catalyst particles.

25. The process of claim 16, wherein the reactor comprises a tapered bed having an upper portion with a diameter greater than a diameter of the lower portion.

26. The process of claim 16, wherein contacting the hydrocarbon reactant with the fluidized bed within the reactor occurs at a temperature between 600-1000 °C.

27. The process of claim 16, wherein the catalyst particles comprise iron, nickel, manganese, cobalt, oxides thereof, ores thereof, and / or combinations thereof.

28. The process of claim 16, further comprising: introducing one or more catalyst promotors into the reactor, wherein the one or more catalyst promotors comprise an alkali metal nitrate, an alkali halide salt, a hydrogen halide, an alkylhalide, a halogen, or a combination thereof.

29. The process of claim 16, wherein the inert particles comprise sand, gravel, magnesia, alumina, zirconia, or any combination thereof.

30. The process of claim 16, wherein the inert particles have a size in a range of between about 0.01 to about 10 mm, and wherein the catalyst particles comprise 1-70 wt.% of a the particle bed.

31. The process of claim 16, wherein the hydrocarbon reactant is contacted with the fluidized bed for a time between 0.1 to 10 seconds.

32. The process of claim 16, wherein the solid carbon is produced at a weight ratio of the solid carbon to the catalyst particles of greater than 7.

33. The process of claim 16, further comprising: exchanging heat between the hydrocarbon and carbon in the upper portion and the hydrocarbon reactants in the lower portion.

34. The process of claim 16, further comprising: contacting the outlet gas with a second particle bed; and exchanging heat with the second particle bed and the inert particles in the lower portion of the reactor.

35. A fluidized bed reaction process comprising: contacting a hydrocarbon reactant with a fluidized bed within a reactor, wherein the fluidized bed comprises catalyst particles, solid carbon, and inert particles, wherein the hydrocarbon reactant comprises an impurity; stratifying the fluidized bed within the reactor, wherein the inert particles move to a lower portion of the fluidized bed, and wherein the solid carbon and catalyst particles move to an upper portion of the fluidized bed; forming the solid carbon and hydrogen based on contacting the hydrocarbon reactant with the fluidized bed; reacting at least a portion of the impurity with a portion of the catalyst particles; and removing the hydrogen and at least a portion of the solid carbon from the reactor.

36. The process of claim 35, further comprising: removing at least a portion of the inert particles from the lower portion of the fluidized bed; combusting at least a portion of the hydrogen to heat the inert particles and form heated inert particles; and passing the heated inert particles to the upper portion of the fluidized bed.

37. The process of claim 35, further comprising: forming the solid carbon on the catalyst particles; and removing a portion of the solid carbon from the catalyst particles using the inert particles.

38. The process of claim 35, further comprising: removing a portion of the catalyst particles from the reactor with the solid carbon; and separating the portion of the catalyst particles from the solid carbon in a separator, wherein the separator comprises a cyclone separator or a magnetic separator.

39. The process of claim 35, further comprising: introducing catalyst precursor particles into the reactor; and converting the catalyst precursor particles into the catalyst particles within the reactor based on contacting the hydrocarbon with the catalyst precursor particles.

40. The process of claim 35, wherein the reactor comprises a tapered bed having an upper portion with a diameter greater than a diameter of the lower portion.

41. The process of claim 35, wherein the catalyst particles comprise iron, nickel, manganese, cobalt, oxides thereof, ores thereof, and / or combinations thereof.

42. The process of claim 35, further comprising: introducing one or more catalyst promotors into the reactor, wherein the one or more catalyst promotors comprise an alkali metal nitrate, an alkali halide salt, a hydrogen halide, an alkylhalide, a halogen, or a combination thereof.

43. The process of claim 35, wherein the inert particles comprise sand, gravel, magnesia, alumina, zirconia, or any combination thereof.

44. The process of claim 35, wherein the solid carbon is produced at a weight ratio of the solid carbon to the catalyst particles of greater than 7.

45. The process of claim 35, wherein the hydrocarbon reactant comprises methane, ethane, natural gas, alkenes, alcohols, pyrolyzed products of a hydrocarbon liquid, or solid hydrocarbons.

Citation Information

Patent Citations

  • Method of biomass grading pyrolysis gasification in a circulating fluidized bed

    US20200224110A1

  • Process of promoting reactions in a fluidized bed comprising a plurality of catalysts

    US2503291A

  • Fluidised bed pyrolysis apparatus and method

    WO2022056559A1

  • Process for converting solid hydrocarbonaceous materials to chemicals and fuels

    WO2023114241A1

  • Systems and methods for hydrocarbon pyrolysis using moving bed and fluidized bed reactors