Equivalent testing method for piston impact tester and rocker-arm impact tester within half-crushing time

By adjusting and calculating the impact time and determining the equivalent test formula, the problem of inconsistent results between the piston impactor and the rocker arm impactor in the half-crushing time test was solved, the test results were unified, and the cost of equipment replacement was avoided. Promoted international trade and academic exchanges.

WO2024212292A1PCT designated stage expired Publication Date: 2024-10-17CHINA NORTH STANDARDIZATION CENT
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/092639
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-13
Filing Date
2023-05-08
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

When conducting half-crushing time tests on piston impact meters and rocker impact meters used in different countries and regions, the test results are inconsistent, resulting in the inability to uniformly evaluate the performance of superabrasives, affecting international and domestic trade, and replacing one type of equipment with another. There is a waste of equipment investment and learning costs in the method of achieving uniform test results.

Method used

By selecting high, medium and low-grade superabrasive samples, setting the standard vibration frequency respectively, estimating and adjusting the impact time, calculating the impact cycle ratio, and determining the equivalent test formula, the comparison between the piston impact meter and the rocker arm impact meter is realized. The test results are uniform.

Benefits of technology

The consistency of the test results of the piston impactor and the rocker arm impactor under the half-crushing time test method is achieved, which avoids economic losses and waste caused by equipment replacement, promotes international trade and academic exchanges of superhard abrasives, and establishes unified quality Assess the environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023092639_17102024_PF_FP_ABST
    Figure CN2023092639_17102024_PF_FP_ABST
Patent Text Reader

Abstract

An equivalent testing method for a piston impact tester and a rocker-arm impact tester within a half-crushing time. Three grades, i.e. a high grade, a medium grade and a low grade of samples of super-hard abrasives having the same size are used as comparison objects of an equivalence relationship between two types of impact testers; by using a half-crushing time method and using a piston impact tester and a rocker arm impact tester, the same sample is impacted, so as to obtain times at which a non-crushing rate of the sample is 50%, and the times are converted into impact cycles; the ratio of half-crushing impact cycles for the samples of the same grade of the piston impact tester and the rocker arm impact tester is calculated, so as to obtain magnitude differences between impact ratios of the two types of impact testers with regard to the samples of the three grades; a deviation range where a relative percentage of the ratio of the impact cycles is located or the degree of linearity of the ratio of the impact cycles between the samples of different grades is determined, so as to determine a calculation scheme for equivalent testing results; equivalent testing results of the two types of impact testers are calculated according to formulas corresponding to the deviation range of the relative percentage; for samples of some sizes with severe non-linearity, the number of grade classifications is increased, so as to implement high-precision equivalence between the two types of impact testers; and according to usage requirements for the testing results, equivalent impact cycles are converted into equivalent impact times.
Need to check novelty before this filing date? Find Prior Art

Description

Equivalent test method for half-breakage time of piston and rocker impact testers Technical Field

[0001] The invention belongs to the technical field of super-hard abrasive impact toughness testing, and particularly relates to an equivalent testing method for half-crushing time of a piston and a rocker impact instrument. Background Art

[0002] Piston impactors and rocker impactors are essential instruments for testing the impact toughness of superabrasives. Superabrasives primarily refer to extremely hard abrasives such as diamond and cubic boron nitride. They are primarily used in cutting tools and grinding tools, forming the core element of these tools. Impact toughness is a key performance indicator of superabrasives. There are two primary methods for testing impact toughness: the half-breakage time test and the unbreakage rate test. These two methods use completely different indicators (evaluation metrics) and calculation formulas. The half-breakage time test uses the length of time, or the number of impact cycles (time can be converted to impact cycles), to measure the impact toughness of a superabrasive. The unbreakage rate test uses the proportion of the unbroken sample to the total sample volume to measure the impact toughness. The calculation complexity of the two test methods differs significantly, and each has its own distinct advantages. The calculation formula and testing steps for the half-breakage time test are significantly more complex than those for the unbreakage rate test. Both methods can be performed using either a piston impactor or a rocker impactor.

[0003] As mentioned above, there are two main types of impact instruments used in the half-crush time test and the uncrushed rate test: a piston impactor and a rocker impactor. The design principles and structures of these two impact instruments are completely different. The piston impactor uses a piston reciprocating motion to impact the abrasive through an impact tube filled with superabrasive. The piston impactor consists of an impact tube 1, an impact tube frame 2, a connecting rod 3, a drive wheel 4, a motor shaft 5, and a piston 6. Its structure is shown in Figure 1. The rocker impactor, on the other hand, uses a rocker reciprocating motion to impact the abrasive through an impact tube filled with superabrasive. The rocker impactor consists of an impact tube 1, an impact tube frame 2, a connecting rod 3, a drive wheel 4, a motor shaft 5, a rocker arm 6', and a rocker arm shaft 7. Its structure is shown in Figure 2. Rocker vibrators and piston vibrators each have their advantages and disadvantages. Rocker vibrators offer the advantages of a high number of impacts and a long operating time, making them suitable for production inspections. However, they are bulky and heavy. The piston vibrator has the advantages of small size and light weight, but it is easy to heat up and difficult to work for a long time. It is suitable for precision testing and arbitration testing.

[0004] The distribution of these two test methods and types of impact instruments varies significantly worldwide. The United States, Europe, and some Asian countries, such as Japan, primarily use the half-breakage time test method, while China primarily uses the unbreakage rate test method. The United States, Japan, and China mostly use rocker impact instruments, with a smaller number using piston impact instruments, while European countries mostly use piston impact instruments, with a smaller number using rocker impact instruments.

[0005] When two different devices are used to test the same superabrasive sample using the same test method (half-crush time method or uncrushed rate method), the results obtained are completely different. This makes it difficult for superabrasive manufacturers and users in different regions of the world to uniformly evaluate the performance of the same abrasive, seriously hindering the unified performance evaluation of superabrasives and the development of international trade.

[0006] The most intuitive approach to unification is to combine the two methods into one, and the two types of equipment into one category. However, since each testing method has its own distinct advantages and has established usage habits among users worldwide, unification is impossible. Furthermore, the two impact instruments used to test superabrasives also have their own performance advantages. Furthermore, users of each type of impact instrument have invested heavily in their own equipment and are accustomed to using their own devices. Therefore, standardizing testing equipment by replacing one with another is also impossible. Therefore, the problem of unifying test results for the same superabrasive specimen using two different types of testing equipment using the same testing method can only be solved through technical means. The issue of equivalent testing methods for the unbroken rate test method using a piston impactor and a rocker impactor has been addressed through the granted patent (Patent No.: ZL 202011497349.2) "Equivalent Testing Methods for Rocker and Piston Vibrators." However, due to the technical complexity of the half-breakage time test method, equivalent testing methods for the same specimen using a piston impactor and a rocker impactor have yet to be found. The half-breakage time test method is the most widely used method in the world, and many countries and companies use this test method to conduct tests using piston impactors and rocker impactors.

[0007] For the same superabrasive sample, the results obtained using the half-breakage time test method using a piston impactor and a rocker impactor can differ significantly. For example, for a high-grade sample of size D426, the piston impactor test yielded a result of 260 seconds, while the rocker impactor test yielded a result of 150 seconds. Using different impact equipment to test the same sample using the same test method yielded different results. This makes it difficult for superabrasive manufacturers and users (such as cutting tool manufacturers) around the world, who utilize different types of testing equipment, to reach a unified assessment of superabrasive performance. Because different superabrasive manufacturers use different types of testing equipment, the product performance indicators they provide are not comparable. Users of superabrasives also struggle to confirm the performance of their supplied abrasives due to differences in equipment with those of the abrasive manufacturers. Abrasives with long half-breakage times provided by manufacturers are not necessarily high-performing, and abrasives with short half-breakage times tested by users are not necessarily low-performing. This lack of uniformity in test results has resulted in inconsistent performance indicators for the procurement and delivery of superabrasive products, severely impacting both domestic and international trade in superabrasives and leading to numerous trade disputes. While retaining the two widely used impactors, achieving equivalence or unification of the half-breakage time test results using two different impactors has become a pressing global technical challenge in the superabrasives industry.

[0008] Summary of the Invention

[0009] (1) Technical issues to be solved

[0010] The technical problem to be solved by the present invention is: to create a method for equivalence of test results using the half-crushing time method for a piston impactor and a rocker impactor, so that the test results of the half-crushing time test method, which is the most widely used method in countries around the world, are consistent when the same specimens are tested using two different impactors, thereby avoiding the waste of equipment investment in a large number of impact testing equipment and the waste of equipment use learning costs in achieving unified test results by replacing one impactor with another, so as to achieve comparability and uniformity of test results of the half-crushing test method worldwide, regardless of whether a piston impactor or a rocker impactor is used.

[0011] (2) Technical solution

[0012] In order to solve the above technical problems, the present invention provides an equivalent test method for the half-crushing time of a piston and a rocker impact instrument, comprising the following steps:

[0013] S1, select the size of S i The samples are divided into three grades: high grade, medium grade and low grade. i represents the brand of super abrasive. At least 4 batches of samples are prepared for each grade.

[0014] S2. Set the standard vibration frequency f of the rocker impact instrument respectively r and the standard vibration frequency f of the piston impact tester p ;

[0015] S3, for the size of S i For samples of high, medium and low grades, estimate the impact time t when the samples are impacted by a rocker impact instrument until the unbroken rate of the samples is between 45% and 50%. rH1 , t rM1 and t rL1 In addition, the impact time t of the high, medium and low grade samples when the piston impact instrument is used to impact the sample until the unbroken rate is in the range of 45% to 50% is estimated. pH1 , t pM1 and t pL1 ;

[0016] S4, respectively, for each rocker arm and piston impact instrument using the estimated corresponding high-grade sample corresponding impact time t rH1 and t pH1 Set the impact time; place a high-grade sample in the impact tube of each impactor, install the impact tube on the impactor, and start each impactor to perform the impact work;

[0017] S5. Screen and weigh the impacted samples respectively to obtain the impact time T for the rocker impact instrument. rH1 Impact unbroken rate P rH1 , impact time T for piston impact tester pH1 Impact unbroken rate P pH1 , P rH1 and P pH1 The unbroken rate value is between 45% and 50%;

[0018] S6. When the unbroken rate of the sample impacted by the rocker impactor or piston impactor is less than 45%, appropriately reduce the impact time of the corresponding sample and use a new identical sample to perform the same impact until the unbroken rate of the sample is between 45% and 50%. At this time, record the impact time T of the rocker impactor respectively. rH1 and the unbroken rate P of the impact specimen rH1 , impact time T of piston impact tester pH1 and the unbroken rate P of the impact specimen pH1 ;

[0019] S7. According to S4 to S6, use two types of impact instruments to impact medium-grade and low-grade samples respectively, and estimate the impact time t rM1 With t pM1 and t rL1 With t pL1, use the corresponding impact instrument to impact, then screen and weigh, and obtain the impact time T of the rocker impact instrument on the medium-grade sample rM1 and the unbroken rate of the sample P rM1 , the impact time T of the piston impact tester on the medium-grade sample pM1 and the unbroken rate of the sample P pM1 , and the impact time T of the rocker impact tester on low-grade samples rL1 and the unbroken rate of the sample P rL1 , the impact time T of the piston impact tester on the low-grade sample pL1 and the unbroken rate of the sample P pL1 ;

[0020] S8. According to steps S1 to S7, use a rocker impactor and a piston impactor to perform impact tests on high-grade, medium-grade and low-grade samples respectively. The unbroken rates of the three grade samples after impact are between 50% and 55%. When the unbroken rate of the samples impacted by the rocker impactor or the piston impactor is greater than 55%, appropriately increase the impact time of the corresponding sample and perform the same impact with a new identical sample until the unbroken rate of the sample is between 50% and 55%. At this time, record the impact time T of the rocker impactor on the three grade samples respectively. rH2 , T rM2 and T rL2 and the unbroken rate P of the corresponding impact specimen rH2 , P rM2 and P rL2 , the impact time T of the piston impact tester on the three grade samples pH2 , T pM2 and T pL2 and the unbroken rate P of the impact specimen pH2 , P pM2 and P pL2 ;

[0021] S9. Use formula (1), formula (2) and formula (3) to calculate the impact time T when the high-grade, medium-grade and low-grade samples are impacted by the rocker impact instrument when the unbroken rate is 50%. rH50 , T rM50 and T rL50 , and then further converted into the corresponding impact cycle C rH50 , C rM50 and C rL50 :

[0022] S10. Use formula (4), formula (5) and formula (6) to calculate the impact time T when the piston impact instrument is used to impact high-grade, medium-grade and low-grade samples when the unbroken rate is 50%.pH50 , T pM50 and T pL50 , and then further converted into the corresponding impact cycle C pH50 , C pM50 and C pL50 :

[0023] S11. Use formula (7), formula (8) and formula (9) to calculate the impact cycles C of the piston impact tester for the three grades of samples respectively. pH50 , C pM50 and C pL50 Apply the impact cycle C of the rocker impact tester to the corresponding grade sample rH50 , C rM50 and C rL50 R H50 , R M50 and R L50 :

[0024] S12. Use formula (10) to calculate the impact cycle ratio R of the three grade samples H50 , R M50 and R L50 The average value r A50 :

[0025] S13. Repeat the parallel test according to steps S1 to S12 using the same sample grade and batch number as in steps S1 to S12. The average of the two parallel tests calculated by the above formula is the result R. A50 ;

[0026] S14. Calculate R A50 Minus R H50 , R M50 or R L50 One divided by R A50 Get three relative percentages. When any of the three relative percentages is not greater than 1.5%, [|R A50 -R x50 | / R A50 =R D50max / R A50 ]≦1.5%,x=H,M or L;R D50max =|R A50 -R x50|, execute step S15; when any one of the three relative percentages is greater than 1.5%, execute step S16; when the three relative percentages are much greater than 1.5%, that is, they reach or exceed the preset threshold, and the expected accuracy is greater than the equivalent test result of the preset value, execute step S17;

[0027] S15. At this time, the equivalent test results of each grade sample using a piston impactor or a rocker impactor are C Epx50 or C Erx50 The calculation does not take into account the relative percentage of the grade relationship, when a sample size specification S i The impact test result of any new sample of any grade using a rocker impact tester or a piston impact tester is C Nrx50 or C Npx50 , equivalent test results C of the same sample impacted by a piston impactor or rocker impactor different from the last impactor Epx50 or C Erx50 Calculate according to formula (11) or formula (12): C Epx50 =R A50 ·C Nrx50 (11)

[0028] S16, at this time any of the three relative percentages is greater than 1.5%, [|R A50 -R x50 | / R A50 =R D50max / R A50 ]>1.5%, the equivalent test results of each grade sample using piston impact instrument or rocker impact instrument C Epx50 or C Erx50 The calculation of the relative percentage of the grade relationship is considered. In this case, the equivalent test result of the piston impactor or rocker impactor on the high-grade sample is C EpH50 or C ErH50 , the equivalent test result of the medium grade sample is C EpM50 or C ErM50 , the equivalent test result of the low-grade sample is C EpL50 or C ErL50 , when a sample size specification S i New samples of medium-high grade, medium grade and low grade are subjected to impact test by rocker impact tester or piston impact tester. The corresponding test results of high grade are C NrH50 or C NpH50 , the middle grade is C NrM50 or C NpM50 and the lower grade is C NrL50 or C NpL50, the equivalent test results of three grades of the same sample tested with a piston impactor or rocker impactor different from the last impactor C EpH50 or C ErH50 , C EpM50 or C ErM50 , C EpL50 or C ErL50 Calculate according to formula (13), formula (14), formula (15), formula (16), formula (17) or formula (18): C EpH50 =R H50 ·C NrH50 (13) C EpM50 =R M50 ·C NrM50 (15) C EpL50 =R L50 ·C NrL50 (17)

[0029] S17. At this time, the three relative percentages are much greater than 1.5%, and the expected accuracy is greater than the preset value of the equivalent test results. The number of grade layers of the test samples of the same size is increased to 5 grades or 7 grades. In this case, refer to steps S1 to S16 to reconstruct the equivalent calculation formulas of 5-grade or 7-grade samples in one size, and then apply these formulas to calculate the equivalent test results between the rocker impact tester and the piston impact tester.

[0030] Preferably, after step S17, the method further includes: step S18, converting the equivalent impact cycles of the three grades of piston impact instrument and rocker impact instrument into equivalent impact time according to formula (19) and formula (20): T Epx50 =C Epx50 ×f p (19) T Erx50 =C Erx50 ×f r (20)

[0031] Thus, equivalent test results can be obtained for each grade of superabrasive samples of the same size tested between the piston impact tester and the rocker impact tester.

[0032] Preferably, after step S18, the method further includes step S19, obtaining equivalent test results of samples of all grades of superhard abrasives of all sizes tested between the piston impact tester and the rocker impact tester.

[0033] The present invention also provides a system for implementing the method.

[0034] The invention also provides an application of the method in the technical field of super-hard abrasive impact toughness testing.

[0035] The present invention also provides an application of the system in the technical field of super-hard abrasive impact toughness testing. (3) Beneficial effects

[0036] The present invention uses high-grade, medium-grade and low-grade samples of superhard abrasives of the same size as comparison objects for the equivalence relationship between two types of impact instruments; adopts the half-crushing time method to use a piston impact instrument and a rocker impact instrument to respectively impact the same sample to obtain the time when the sample has a 50% uncrushed rate, and converts the time into impact cycles; calculates the ratio of the half-crushing impact cycles of the same grade samples of the piston impact instrument and the rocker impact instrument to obtain the difference in the impulse ratio of the two types of impact instruments on the three grade samples; judges the deviation range of the relative percentage of the impact cycle ratio or the linearity of the impact cycle ratio between samples of each grade to determine the calculation scheme of the equivalent test results; calculates the equivalent test results of the two types of impact instruments according to the formula corresponding to the comparison percentage deviation range; for certain size samples with severe nonlinearity, increases the number of grades for grade division to achieve high-precision equivalence of the two types of impact instrument tests; and converts the equivalent impact cycles into equivalent impact time according to the needs of using the test results. Based on the above technical solution, the present invention solves the global technical problem that the half-crushing time method uses a piston impactor and a rocker impactor to test the same sample differently, so that the world's most widely used half-crushing time test method can achieve the same test results for the same superabrasive sample using a piston impactor and a rocker impactor that are completely different in working principle and structure, so that the test results of different impact equipment users can be unified, avoiding the contradictions and disputes caused by inconsistent test results in the international trade of superabrasives, and also avoiding the economic losses and waste caused by replacing another impact tester with a certain impact tester. This equivalence method also has the advantage that after the sample is tested on one impact tester, the equivalence to another impact tester can be obtained by calculation, eliminating the costs of labor, time, sample and equipment wear caused by testing on another impact tester. The present invention unifies the test results of different test equipment, which will be conducive to promoting the development of international trade, promoting academic exchanges in the field of superabrasives, and establishing a good environment for international evaluation of the quality of superabrasives. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] FIG1 is a structural diagram of a piston impact instrument;

[0038] Figure 2 is a structural diagram of a rocker impact tester;

[0039] FIG3 is a graph showing the relationship between the impact cycles and the percentage ratio of no more than 1.5% in the present invention;

[0040] FIG4 is a graph showing the relationship between the impact cycles and the percentage ratio greater than 1.5% in the present invention;

[0041] FIG. 5 is a graph showing the relationship between the impact cycles and the percentage ratio far greater than 1.5% in the present invention. DETAILED DESCRIPTION

[0042] In order to make the purpose, content and advantages of the present invention more clear, the specific implementation methods of the present invention are further described in detail below with reference to the accompanying drawings and examples.

[0043] The inventors of the present invention discovered that for samples of three grades of the same particle size, namely high grade, medium grade and low grade, the half-crushing time and corresponding half-crushing impact cycles of the same three grades of samples were measured using a piston impactor and a rocker impactor using a half-crushing time test method, the corresponding half-crushing impact cycle ratios of the three grades of samples measured by the piston impactor and the rocker impactor were calculated, the average value of the half-crushing impact cycle ratios of the three grades of samples was calculated, the relative percentage of the half-crushing impact cycle ratio was calculated, the deviation limit value of the relative percentage of the half-crushing impact cycle ratio was set (for example, 1.5% or 2%, etc.), and the relative percentage of the half-crushing impact cycle ratio of the three grades of test samples was compared with the deviation limit value, so as to evaluate the linearity of the impulse ratio of the piston impactor and the rocker impactor for the tested size samples at the three grades. Further, the type of formula used in the equivalent calculation is determined according to the linearity state of the impulse ratio. If the linearity state of the impulse ratio is good, the equivalent test value is calculated by taking the average value of the relative percentage of the semi-crushing impact cycle ratio. If the linearity state of the impulse ratio is not good, the equivalent test value is calculated by taking the relative percentage of the semi-crushing impact cycle ratio of the three grades of samples respectively. In this way, the equivalent test results of each grade of superhard abrasives of the same size tested between the piston impact tester and the rocker impact tester can be obtained.

[0044] According to the above inventive ideas, the equivalent testing method of the present invention specifically includes the following steps:

[0045] S1, select the size of S i (i represents the brand of super abrasive, i=D851,…,D46,B301,…,B46, for example S D426 =40 / 45, with the brand name D426) samples of three grades: high, medium, and low. Prepare at least four or more batches of samples for each grade (a total of 3 x 4 = 12 or more batches for the three grades).

[0046] S2. Select and set the standard vibration frequency f of the rocker impact instrument r and the standard vibration frequency f of the piston impact tester p , for example, f r =2 400r / min,fp =1 420r / min.

[0047] S3, for the size of S i For samples of high, medium and low grades, estimate the impact time t when the samples are impacted by a rocker impact instrument until the unbroken rate of the samples is between 45% and 50%. rH1 , t rM1 and t rL1 In addition, the impact time t of the high, medium and low grade samples when the piston impact instrument is used to impact the sample until the unbroken rate is between 45% and 50% is estimated. pH1 , t pM1 and t pL1 .

[0048] S4, respectively, for each rocker arm and piston impact instrument using the estimated corresponding high-grade sample corresponding impact time t rH1 and t pH1 Set the impact time. Place a high-grade sample in the impact tube of each impactor, install the impact tube on the impactor, and start each impactor to perform the impact.

[0049] S5. Screen and weigh the impacted samples respectively to obtain the impact time T for the rocker impact instrument. rH1 Impact unbroken rate P rH1 , impact time T for piston impact tester pH1 Impact unbroken rate P pH1 (P rH1 and P pH1 The unbroken rate is between 45% and 50%).

[0050] S6. When the unbroken rate of the sample impacted by the rocker impactor or piston impactor is less than 45%, appropriately reduce the impact time of the corresponding sample and use a new identical sample to perform the same impact until the unbroken rate of the sample is between 45% and 50%. At this time, record the impact time T of the rocker impactor and the impact time T of the piston impactor respectively. rH1 and the unbroken rate P of the impact specimen rH1 , impact time T of piston impact tester pH1 and the unbroken rate P of the impact specimen pH1 .

[0051] S7. According to S4 to S6, use two types of impact instruments to impact medium-grade and low-grade samples respectively, and estimate the impact time t rM1 With t pM1 and t rL1 With t pL1 , use the corresponding impact instrument to impact, then screen and weigh, and obtain the impact time T of the rocker impact instrument on the medium-grade sample rM1 and the unbroken rate of the sample PrM1 , the impact time T of the piston impact tester on the medium-grade sample pM1 and the unbroken rate of the sample P pM1 , and the impact time T of the rocker impact tester on low-grade samples rL1 and the unbroken rate of the sample P rL1 , the impact time T of the piston impact tester on the low-grade sample pL1 and the unbroken rate of the sample P pL1 .

[0052] S8. According to S1 to S7, use the rocker impactor and piston impactor to conduct impact tests on high-grade, medium-grade and low-grade samples respectively. The unbroken rate of the three grade samples after impact is between 50% and 55%. When the unbroken rate of the samples impacted by the rocker impactor or piston impactor is greater than 55%, appropriately increase the impact time of the corresponding samples and use new identical samples to perform the same impact until the unbroken rate of the samples is between 50% and 55%. At this time, record the impact time T of the rocker impactor impacting the three grade samples respectively. rH2 , T rM2 and T rL2 and the unbroken rate P of the corresponding impact specimen rH2 , P rM2 and P rL2 , the impact time T of the piston impact tester on the three grade samples pH2 , T pM2 and T pL2 and the unbroken rate P of the impact specimen pH2 , P pM2 and P pL2 .

[0053] S9. Use formula (1), formula (2) and formula (3) to calculate the impact time T when the high-grade, medium-grade and low-grade samples are impacted by the rocker impact instrument when the unbroken rate is 50%. rH50 , T rM50 and T rL50 , and then further converted into the corresponding impact cycle C rH50 , C rM50 and C rL50 .

[0054] S10. Use formula (4), formula (5) and formula (6) to calculate the impact time T when the piston impact instrument is used to impact high-grade, medium-grade and low-grade samples when the unbroken rate is 50%. pH50 , T pM50 and T pL50 , and then further converted into the corresponding impact cycle C pH50 , CpM50 and C pL50 .

[0055] S11. Use formula (7), formula (8) and formula (9) to calculate the impact cycles C of the piston impact tester for the three grades of samples respectively. pH50 , C pM50 and C pL50 Apply the impact cycle C of the rocker impact tester to the corresponding grade sample rH50 , C rM50 and C rL50 R H50 , R M50 and R L50 .

[0056] S12. Use formula (10) to calculate the impact cycle ratio R of the three grade samples H50 , R M50 and R L50 The average value r A50 .

[0057] S13. Repeat the parallel test according to S1 to S12 using the same sample grade and batch number as S1 to S12.

[0058] The result of the above formula is calculated by taking the average of two parallel tests as the result R A50 .

[0059] S14. Calculate R A50 Minus R H50 , R M50 or R L50 One divided by R A50 Three relative percentages are obtained, {For example, the relative percentage of the impact cycle ratio of high-grade samples is calculated using the formula [(R A50 -R H50 ) / R A50 ] means}. When any of the three relative percentages is not greater than 1.5%, {[|R A50 -R x50 | / R A50 =R D50max / R A50 ]≦1.5%,x=H,M or L;R D50max =|R A50 -R x503, execute step S15; when any one of the three relative percentages is greater than 1.5%, execute step S16; when the three relative percentages are much greater than 1.5%, reach and exceed 3.0%, and a high-precision equivalent test result is desired, execute step S17;

[0060] S15. At this time, the equivalent test results of each grade sample using a piston impactor or a rocker impactor are C Epx50 or C Erx50 The calculation does not need to consider the relative percentage of the grade relationship. i The impact test result of any new sample of any grade using a rocker impact tester or a piston impact tester is C Nrx50 or C Npx50 , equivalent test results C of the same sample impacted by a piston impactor or rocker impactor different from the last impactor Epx50 or C Erx50 Calculate according to formula (11) or formula (12) respectively. Epx50 =R A50 ·C Nrx50 (11)

[0061] S16, at this time any of the three relative percentages is greater than 1.5% {[|R A50 -R x50 | / R A50 =R D50max / R A50 ]>1.5%,x=H,M or L;R D50max =|R A50 -R x50 |}, as shown in Figure 4, the equivalent test results of each grade sample using a piston impactor or a rocker impactor C Epx50 or C Erx50 The calculation of the relative percentage of the grade relationship needs to be considered. In this case, the equivalent test result of the piston impactor or rocker impactor on the high-grade sample is C EpH50 or C ErH50 , the equivalent test result of the medium grade sample is C EpM50 or C ErM50 , the equivalent test result of the low-grade sample is C EpL50 or C ErL50 When a sample size specification S i New samples of medium-high grade, medium grade and low grade are subjected to impact test by rocker impact tester or piston impact tester. The corresponding test results of high grade are C NrH50 or C NpH50 , the middle grade is C NrM50 or CNpM50 and the lower grade is C NrL50 or C NpL50 , the equivalent test results of three grades of the same sample tested with a piston impactor or rocker impactor different from the last impactor C EpH50 or C ErH50 , C EpM50 or C ErM50 , C EpL50 or C ErL50 Calculate according to formula (13), formula (14), formula (15), formula (16), formula (17) or formula (18). EpH50 =R H50 ·C NrH50 (13) C EpM50 =R M50 ·C NrM50 (15) C EpL50 =R L50 ·C NrL50 (17)

[0062] S17: If the three relative percentages are significantly greater than 1.5% and highly accurate equivalent test results are desired, the number of grade layers for the same-sized test sample should be increased to five or seven grades, as shown in Figure 5. In this severely nonlinear relative percentage situation, refer to S1 through S16 to reconstruct highly accurate equivalent calculation formulas for five or seven grades of the same size. These formulas are then applied to calculate equivalent test results between the rocker impactor and the piston impactor.

[0063] S18. Parameters related to equivalent testing between piston impactors and rocker impactors (e.g., C rH50 , C rM50 , C rL50 , C pH50 , C pM50 , C pL50 , R A50 , R H50 , R M50 , R L50 After the establishment of the impact test method, the equivalent test results of a new sample of a certain sample size using one impact tester and another impact tester can be obtained by calculation, without the need for actual measurement. In this equivalent test method, the equivalent test results of the impact cycle can be converted into the equivalent test time, and the two can be converted into each other. The equivalent impact cycle of the three grades of piston impact tester and rocker impact tester is converted into the equivalent impact time according to formula (19) and formula (20). Epx50 =CEpx50 ×f p (19) T Erx50 =C Erx50 ×f r (20)

[0064] The equivalent test method established using the half-breakage time test method can be used to obtain equivalent test results between piston impactors and rocker impactors for samples of the same size of superabrasives of various grades.

[0065] S19, obtain the equivalent test results of all grades of super abrasives in all sizes between the piston impact tester and the rocker impact tester. D851 ~S D46 and S B301 ~S B46 After the relevant parameters for equivalent testing between the piston impact tester and the rocker impact tester are established, this test method will be generally applicable to the equivalent testing of superhard abrasives of various sizes.

[0066] The test method of the present invention has been verified through actual test experiments. The test data are shown in Table 1. The test verifies that the effect of the present invention is very good. The test uses a diamond sample of size D426, and the weight of each impact is 0.4g. The test samples are high-grade, medium-grade and low-grade samples. The half-crushing time method is used in the test to test and measure the half-crushing time and half-crushing cycle of the three grade samples using a piston impact instrument and a rocker impact instrument, and calculate the impact cycle ratio R of the three grade samples. x50 , average weekly ratio R A50 And the relative percentage of the number of impact cycles. Since the relative percentages of the three grade samples are 0.0%, -2.9% and 1.9% respectively, and two of the three values ​​are greater than 1.5%, the formula for the equivalent test of the two impact instruments should be solved by grade. Some samples of the three grades of D426, high, medium and low, are newly taken and tested by the rocker impact instrument and the piston impact instrument respectively using the half-crushing time method. The rocker impact instrument test results are calculated using the invented algorithm to obtain the equivalent test results of the piston impact instrument. Then, the equivalent test results of the piston impact instrument are subtracted from the results of the actual measured samples of the piston impact instrument (C Epx50 -C Npx50 ), the calculated equivalent differences are very small compared to the measured differences. The differences between the three grades are -62(r), 8(r) and 49(r), respectively. Their percentages in the measured values ​​are -0.9%, 0.1% and 0.9%, respectively, which are significantly lower than the test accuracy requirement of 1.5% (excluding positive and negative numbers, and compared in absolute values).

[0067] Table 1 Verification test of the equivalent test method of piston impact instrument and rocker impact instrument using the half-breakage time method

[0068] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. An equivalent test method for half-crushing time of a piston and a rocker impact instrument, characterized in that: The following steps are involved: S1, select the size S i There are three grades of samples: high grade, medium grade and low grade. i represents the brand of super abrasive. At least 4 batches of samples are prepared for each grade. S2. Set the standard vibration frequency f of the rocker impact instrument respectively r and the standard vibration frequency f of the piston impact instrument p ; S3, for size S i For samples of high, medium and low grades, the impact time t is estimated when the samples are impacted by a rocker impact instrument until the unbroken rate of the samples is between 45% and 50%. rH1 , t rM1 and t rL1 In addition, the impact time t of the high, medium and low grade samples when the piston impact instrument is used to impact the sample until the unbroken rate is between 45% and 50% is estimated. pH1 , t pM1 and t pL1 ; S4, respectively, the rocker arm and piston impact instrument use the estimated corresponding high-grade sample corresponding impact time t rH1 and t pH1 Set the impact time; put a high-grade sample in the impact tube of each impact instrument, install the impact tube on the impact instrument, and start each impact instrument to perform impact work; S5. Screen and weigh the impacted samples respectively to obtain the impact time T for the rocker impact instrument. rH1 Impact unbroken rate P rH1 , Piston impact tester impact time T pH1 Impact unbroken rate P pH1 , P rH1 and P pH1 The unbroken rate value is between 45% and 50%; S6. When the unbroken rate of the samples impacted by the rocker impactor or piston impactor is less than 45%, appropriately reduce the impact time of the corresponding samples and use new identical samples to perform the same impact until the unbroken rate of the samples is between 45% and 50%. At this time, record the impact time T of the rocker impactor respectively. rH1 and the unbroken rate P of the impact specimen rH1 , impact time T of piston impact instrument pH1 and the unbroken rate P of the impact specimen pH1 ; S7. According to S4-S6, use two types of impact instruments to impact the estimated impact time t using medium-grade and low-grade samples respectively. rM1 With t pM1 and t rL1 With t pL1 , use the corresponding impact instrument to impact, then screen and weigh, and obtain the impact time T of the rocker impact instrument on the medium-grade sample rM1 and the unbroken rate of the sample P rM1 , the impact time T of the piston impact tester on the medium-grade sample pM1 and the unbroken rate of the sample P pM1 , and the impact time T of the rocker impact tester on the low-grade sample rL1 and the unbroken rate of the sample P rL1 , the impact time T of the piston impact tester on the low-grade sample pL1 and the unbroken rate of the sample P pL1 ; S8. According to steps S1 to S7, use a rocker impactor and a piston impactor to perform impact tests on high-grade, medium-grade and low-grade samples respectively. The unbroken rates of the three grades of samples after impact are between 50% and 55%. When the unbroken rate of the samples impacted by the rocker impactor or the piston impactor is greater than 55%, appropriately increase the The impact time of the corresponding sample is measured by using a new sample of the same quality until the unbroken rate of the sample is between 50% and 55%. At this time, the impact time T of the rocker impact instrument on the three grades of samples is recorded respectively. rH2 , T rM2 and T rL2 and the unbroken rate P of the corresponding impact specimen rH2 , P rM2 and P rL2 , the impact time T of the piston impact instrument impacting the three grade samples pH2 , T pM2 and T pL2 and the unbroken rate P of the impact specimen pH2 , P pM2 and P pL2 ; S9. Use formula (1), formula (2) and formula (3) to calculate the impact time T of high-grade, medium-grade and low-grade samples when the unbroken rate is 50% using the rocker impact instrument. rH50 , T rM50 and T rL50 , and then further converted into the corresponding impact cycle C rH50 , C rM50 and C rL50 : S10, using formula (4), formula (5) and formula (6), respectively calculate the corresponding impact time T when the unbroken rate of high-grade, medium-grade and low-grade samples is 50% using the piston impact instrument pH50 , T pM50 and T pL50 , and then further converted into the corresponding impact cycle C pH50 , C pM50 and C pL50 : S11. Use formula (7), formula (8) and formula (9) to calculate the impact cycles C of the three grade samples using the piston impact tester. pH50 , C pM50 and C pL50 The number of impact cycles C of the rocker impact tester applied to the corresponding grade samples rH50 , C rM50 and C rL50 R H50 , R M50 and R L50 : S12. Use formula (10) to calculate the impact cycle ratio R of the three grade samples H50 , R M50 and R L50 The average value r A50 : S13, according to steps S1 to S12, repeat the parallel test with the same sample grade and batch number as in steps S1 to S12, and take the average of the two parallel tests as the result R A50 ; S14. Calculate R A50 Minus R H50 , R M50 or R L50 One divided by R A50 Get three relative percentages. When any of the three relative percentages is not greater than 1.5%, [|R A50 -R x50 | / R A50 =R D50max / R A50 ]≦1.5%,x=H,M or L;R D50max =|R A50 -R x50 |, execute step S15; when any one of the three relative percentages is greater than 1.5%, execute step S16; when the three relative percentages are much greater than 1.5%, that is, they reach or exceed the preset threshold, and the expected accuracy is greater than the equivalent test result of the preset value, execute step S17; S15. At this time, the equivalent test results of each grade of samples using a piston impactor or a rocker impactor are C Epx50 or C Erx50 The calculation does not take into account the relative percentage of the grade relationship, when a sample size specification S i The impact test result of any new sample of any grade using a rocker impact tester or a piston impact tester is C Nrx50 or C Npx50 , equivalent test results C of the same sample impacted by a piston impactor or rocker impactor different from the last impactor Epx50 or C Erx50 Calculate according to formula (11) or formula (12): C Epx50 =R A50 ·C Nrx50 (11) S16, at this time any of the three relative percentages is greater than 1.5%, [|R A50 -R x50 | / R A50 =R D50max / R A50 ]>1.5%, the equivalent test results of each grade of samples using piston impact instrument or rocker impact instrument impact impact C Epx50 or C Erx50 The calculation of the relative percentage of the grade relationship is considered. In this case, the equivalent test result of the piston impact tester or rocker impact tester on the high-grade sample is C EpH50 or C ErH50 , the equivalent test result of the medium grade sample is C EpM50 or C ErM50 , the equivalent test result of the low-grade sample is C EpL50 or C ErL50 , when a sample size specification S i New samples of medium-high grade, medium grade and low grade are subjected to impact test by rocker impact tester or piston impact tester. The corresponding test results of high grade are C NrH50 or C NpH50 , the middle grade is C NrM50 or C NpM50 and the lower grade is C NrL50 or C NpL50 , equivalent test results of three grades of the same sample tested with a piston impactor or rocker impactor different from the last impactor C EpH50 or C ErH50 , C EpM50 or C ErM50 , C EpL50 or C ErL50 Calculate according to formula (13), formula (14), formula (15), formula (16), formula (17) or formula (18): C EpH50 =R H50 ·C NrH50 (13) C EpM50 =R M50 ·C NrM50 (15) C EpL50 =R L50 ·C NrL50 (17) S17. At this time, the three relative percentages are much greater than 1.5%, and the expected accuracy is greater than the preset value of the equivalent test results. The grade layers of the test samples of the same size are increased to 5 grades or 7 grades. In this case, refer to steps S1 to S16 to rebuild the equivalent calculation formulas for 5-grade or 7-grade samples in one size, and then apply these formulas to calculate the equivalent test results between the rocker impact tester and the piston impact tester.

2. The method according to claim 1, characterized in that After step S17, the following further comprises: step S18, converting the equivalent impact cycles of the three grades of the piston impact instrument and the rocker impact instrument into equivalent impact time according to formula (19) and formula (20): T Epx50 =C Epx50 ×f p (19) T Erx50 =C Erx50 ×f r (20) Thus, equivalent test results can be obtained for each grade of super-hard abrasive samples of the same size tested between the piston impact tester and the rocker impact tester.

3. The method according to claim 2, characterized in that After step S18, the method further includes step S19, obtaining equivalent test results of samples of all grades of superhard abrasives of all sizes tested between the piston impactor and the rocker impactor.

4. The method according to claim 1, characterized in that i=D851,…,D46,B301,…,B46.

5. The method according to claim 1, characterized in that In step S2, set f r =2 400r / min.

6. The method according to claim 1, characterized in that In step S2, set f p =1 420r / min.

7. The method according to claim 1, characterized in that When the three relative percentages are much greater than 1.5%, that is, reach or exceed 3.0%, and the expected accuracy is greater than the equivalent test result of the preset value, step S17 is executed.

8. A system for implementing the method according to any one of claims 1 to 7.

9. Application of the method according to any one of claims 1 to 7 in the technical field of super abrasive impact toughness testing.

10. Application of the system as claimed in claim 8 in the technical field of super abrasive impact toughness testing.

Citation Information

Patent Citations

  • Diamond compact impact toughness testing and evaluating method

    CN103076244A

  • Method for correcting test value of impact toughness of artificial diamond

    CN104075935A

  • Equivalent test method for rocker arm type and piston type vibration meters

    CN112557174A

  • Manganese dioxide and reduction coal mixing and crushing system

    CN113877666A

  • Impact toughness detecting instrument for particulate brittleness materials

    CN2111522U