Hot dipping and high-temperature austenitizing technologies-based zinc-aluminum-magnesium coated steel sheet to be stamped, preparation method therefor and use thereof

By regulating the Zn-Al-Mg immersion plating solution and high-temperature austenitization process, a eutectic structure and an intermediate compound layer are formed, which solves the problems of cracks and corrosion resistance of zinc-based coatings in hot stamping and improves the performance of zinc-aluminum-magnesium coatings. High temperature mechanical properties and corrosion resistance of steel plates.

WO2024212409A1PCT designated stage expired Publication Date: 2024-10-17BENGANG STEEL PLATES CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/112570
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-10
Filing Date
2023-08-11
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing zinc-based coatings are prone to cracks during the hot stamping process, resulting in brittle fracture of the matrix, and uneven microscopic distribution of coating components leading to high-temperature cracking. It is difficult to control the Zn/Al/Zn2Mg ternary eutectic structure and zinc element enrichment, which affects Corrosion resistance.

Method used

By regulating the composition of the Zn-Al-Mg immersion plating solution and the hot-dip plating process, a complete eutectic structure is formed. Combined with the high-temperature austenitization process, the MgZn2 phase is generated to improve the corrosion resistance of the coating, and Zn is controlled during the hot stamping process. The diffusion of elements forms a Fe-Al or Fe-Al-Zn intermediate compound layer to inhibit crack propagation.

Benefits of technology

The high-temperature tensile mechanical properties and corrosion resistance of zinc-aluminum-magnesium coated steel sheets are significantly improved, the elongation is increased by 7.4%, the corrosion current density is reduced by 0.5×10-5A/cm2, and the cost of raw materials is reduced, making it easy for commercial promotion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023112570_17102024_PF_FP_ABST
    Figure CN2023112570_17102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention discloses a zinc-aluminum-magnesium coated steel sheet based on hot dipping and high-temperature forming technologies, a preparation method therefor and a use thereof. The steel sheet is prepared by hot dipping, austenitizing under high temperature conditions, and stamping. A dip plating solution for the hot dipping is a Zn-Al-Mg dip plating solution, the components are located at a zinc-rich angle of a Zn-Al-Mg ternary phase diagram, and the mass percentage satisfies that the content of Zn is 85-95 wt.%, the content of Al is 4.5-8.5 wt.%, and the content of Mg is 1-4.5 wt.%. After having undergoing hot dipping, the steel sheet is changed into a zinc-aluminum-magnesium coated steel sheet that is composed of a steel sheet, a zinc-aluminum-magnesium coating-2 and an intermediate compound layer, wherein the zinc-aluminum-magnesium coating comprises Zn, Al and MgZn2 phases; the zinc-aluminum-magnesium coating comprises Zn-Al two-phase eutectic and Zn-Al-MgZn2 three-phase eutectic; and the intermediate compound layer is an Fe-Al or Fe-Al-Zn intermetallic compound. After having undergoing austenitizing, the zinc-aluminum-magnesium coated steel sheet is changed into a steel sheet to be stamped that is composed of a steel sheet and a zinc-aluminum-magnesium coating-3, wherein the zinc-aluminum-magnesium coating-3 comprises an α-Fe(Zn, Al) phase. The zinc-aluminum-magnesium coated steel sheet has the corrosion current density Icorr of (1.20-1.68)×10-5A / cm2 as a corrosion-resistant material, and has the elongation of 38-54% as a high-temperature mechanical material.
Need to check novelty before this filing date? Find Prior Art

Description

A zinc-aluminum-magnesium coated steel plate to be stamped based on hot-dip coating and high-temperature austenitization technology, and its preparation method and application Technical Field

[0001] The present invention relates to coated steel for automobiles, and in particular to a zinc-aluminum-magnesium coated steel plate to be stamped based on hot-dip plating and high-temperature austenitization technology, and a preparation method and application thereof. Technical Background

[0002] Hot-dip coating technology for steel plates has the advantages of preventing oxidation and decarburization of the steel plate surface during hot stamping. The coatings used mainly include Al-Si coating, pure Zn coating, Zn-based alloy coating, etc. Among them, Al-Si coating is currently the most widely used, which can effectively prevent oxidation and decarburization of the steel plate surface. However, this type of coating has the problem of poor corrosion resistance to cuts and perforations. Compared with Al-Si coating, zinc-based coating not only has the function of preventing oxidation and decarburization of the steel plate surface, but also has the function of cathodic protection, that is, excellent perforation corrosion resistance and cut corrosion resistance. However, the current zinc-based coating has the technical problem of cracks generating and extending to the substrate during the hot stamping process. This technical problem directly limits the application of zinc-based coating in the field of automobile manufacturing.

[0003] The cause of the above problems, according to the existing literature 1 (Li Xuetao, Zhang Jie, Jiang Sheming, et al. Crack generation and expansion during the forming process of galvanized hot stamping steel plate [J]. Metal Heat Treatment, 2019, 44(03): 202-6.), is that the cause of cracks during the deformation of pure zinc-coated hot stamping steel is the presence of a large amount of Zn element enrichment in the pure zinc coating. Under the synergistic effect of high temperature and external stress, liquid zinc diffuses along the austenite grain boundary and continuously produces α-Fe(Zn) with the substrate. The cracks continue to expand along the interface between α-Fe(Zn) and the liquid phase, resulting in brittle fracture of the substrate.

[0004] Based on the above reasons, the method of adding alloy elements such as Al and Ni to the pure zinc plating solution can be adopted to generate an alloy inhibition layer such as Fe2Al5 at the coating-substrate interface to keep the enriched liquid zinc element away from the substrate and inhibit the diffusion of zinc element into the substrate.

[0005] However, in the existing literature 2 (Cui Qingling, Li Jianping, Li Shiyu, et al. Microstructure evolution and crack formation during heating of zinc-based coating of 22MnB5 steel [J]. Journal of Iron and Steel Research, 2019, 31(02): 227-32.), during the austenitization process, all the Al elements in the Fe2Al5 alloy inhibition layer of the GI coating plate migrate to the coating surface, the Fe2Al5 alloy layer disappears, the inhibition effect fails, and a large amount of locally enriched zinc elements in the coating diffuse into the matrix, causing brittle fracture of the matrix.

[0006] To address the above issues, existing document 3 (CN107099748B[P].2019) discloses an ultra-high-strength zinc-aluminum-magnesium coated steel sheet for high-temperature forming and a method for manufacturing the same. The coating before high-temperature forming comprises three structures: a Zn / Al eutectic structure, a Zn / Al / Zn2Mg ternary eutectic structure, and pure Zn particles. However, this technology still has the following problems: the content of the Zn / Al / Zn2Mg ternary eutectic structure and the enrichment of zinc in the coating alloy are difficult to control, and the high-temperature reaction of the locally enriched zinc with the steel substrate is difficult to suppress, resulting in high-temperature cracking of the hot-dip galvanized steel sheet.

[0007] Summary of the Invention

[0008] The purpose of the present invention is to provide a zinc-aluminum-magnesium coated steel sheet to be stamped based on hot-dip plating and high-temperature austenitization technology and a preparation method thereof. In order to solve the problem of high-temperature cracking caused by the uneven microscopic distribution of the coating components mentioned in the background technology, a complete eutectic structure is formed by regulating the plating solution composition and the hot-dip plating process, thereby improving the microscopic component segregation and local enrichment of the Zn element in the coating; regulating the austenitization process parameters and the hot stamping process parameters, thereby suppressing the high-temperature cracking of the hot-dip galvanized steel sheet; at the same time, the low-potential phase MgZn2 generated by the reaction of the Mg element added when regulating the plating solution composition and the Zn element can greatly improve the corrosion resistance of the coating.

[0009] The specific technical solutions of the present invention are as follows:

[0010] The present invention provides a zinc-aluminum-magnesium coated steel plate to be stamped based on hot-dip plating and high-temperature austenitizing technology, wherein the steel plate is prepared by hot-dip plating and austenitizing under high-temperature conditions;

[0011] The hot-dip plating solution is a Zn-Al-Mg plating solution, and the specific mass percentages of the components of the Zn-Al-Mg plating solution meet the following requirements: Zn content is 85-95 wt.%, Al content is 4.5-8.5 wt.%, and Mg content is 1-4.5 wt.%.

[0012] The steel plate becomes a zinc-aluminum-magnesium coated steel plate based on hot-dip coating technology after hot-dip coating. The zinc-aluminum-magnesium coated steel plate based on hot-dip coating technology is composed of a steel plate, a zinc-aluminum-magnesium coating-2, and an intermediate compound layer between the steel plate and the coating, wherein:

[0013] The zinc-aluminum-magnesium coating-2 comprises Zn, Al, and MgZn2 phases; the zinc-aluminum-magnesium coating-2 comprises a Zn-Al two-phase eutectic and a Zn-Al-MgZn2 three-phase eutectic;

[0014] In the Zn-Al two-phase eutectic and the Zn-Al-MgZn2 three-phase eutectic of the zinc-aluminum-magnesium coating-2, the total eutectic content of the Zn-Al two-phase eutectic and the Zn-Al-MgZn2 three-phase eutectic is 50-95%, the Zn element exists in the form of Zn phase and MgZn2 phase, and the interlamellar spacing of the eutectic structure is less than 1 micron;

[0015] The intermediate compound layer between the steel plate and the coating, referred to as the intermediate compound layer, is an Fe-Al or Fe-Al-Zn intermetallic compound;

[0016] The zinc-aluminum-magnesium coated steel sheet based on the hot-dip coating technology is austenitized at 900-920° C. to become a zinc-aluminum-magnesium coated steel sheet to be stamped based on the hot-dip coating and high-temperature austenitization technology.

[0017] The zinc-aluminum-magnesium coated steel plate to be stamped based on hot-dip coating and high-temperature austenitizing technology is composed of a steel plate and a zinc-aluminum-magnesium coating-3, wherein the zinc-aluminum-magnesium coating-3 is composed of an α-Fe (Zn, Al) single-layer structure, in which Fe, Zn, Al and Mg elements are evenly distributed, with a Zn element content of 3.5-10.3wt.%, an Al element content of 0.5-12.2wt.%, a Mg element content of 0-0.2wt.%, and an O element content of 0.5-8.2wt.%.

[0018] Furthermore, in the above technical solution, the mass percentages of the steel plate components are as follows: C content is 0.31-0.35wt.%, Si content is 0.05-0.20wt.%, Mn content is 1.40-1.50wt.%, P content is not more than 0.020wt.%, S content is not more than 0.004wt.%, Al content is not less than 0.060wt.%, Ti content is 0.010-0.025wt.%, V content is 0.16-0.20wt.%, N content is not more than 0.0045wt.%, B content is 0.0010-0.0030wt.%, and the remainder is Fe and unavoidable impurities;

[0019] Furthermore, in the above technical solution, in the Zn-Al two-phase eutectic and the Zn-Al-MgZn2 three-phase eutectic of the zinc-aluminum-magnesium coating-2, the Zn element exists in the form of Zn phase and MgZn2 phase, and the Al element exists in the form of Al phase; the interlamellar spacing of the eutectic structure is less than 1 micron.

[0020] Furthermore, in the above technical solution, the thickness of the intermediate compound layer is 0.3-3 microns.

[0021] Furthermore, in the above technical solution, the Zn content in the immersion plating solution is 85-95 wt.%; the composition of the Zn-Al-Mg immersion plating solution is located at the zinc-rich corner of the Zn-Al-Mg ternary phase diagram.

[0022] The present invention provides a method for preparing a steel plate to be stamped with a zinc-aluminum-magnesium coating based on hot-dip coating and high-temperature austenitization technology, comprising the following steps:

[0023] Step 1, preparation of a steel plate to be hot-dip coated;

[0024] Step 2, hot-dip plating of the steel sheet to be hot-dip plated, first preparing a plating solution, and then hot-dip plating the steel sheet to be hot-dip plated obtained in step 1, thereby obtaining a zinc-aluminum-magnesium coated steel sheet based on hot-dip plating technology, named Sample 1-2;

[0025] In step 2, the mass percentage of the immersion plating solution is: Al content is 4.5-8.5wt.%, Mg content is 1-4.5wt.%, and the rest is Zn and unavoidable impurities;

[0026] In step 2, the hot-dip coating conditions are as follows: the coating temperature is 440-460° C., the coating time is 3-10 seconds, and the cooling rate after the coating is completed is greater than 30° C. / s to cool to room temperature;

[0027] Step 3, austenitizing the zinc-aluminum-magnesium coated steel sheet based on hot-dip coating technology, austenitizing the sample 1-2 obtained in step 2, that is, obtaining a zinc-aluminum-magnesium coated steel sheet to be stamped based on hot-dip coating and high-temperature austenitizing technology, named sample 1-3;

[0028] In step 3, the austenitizing conditions are: an austenitizing temperature of 900-920° C. and a holding time of 1-3 minutes;

[0029] The present invention provides a stamping forming method for the zinc-aluminum-magnesium coated steel plate to be stamped based on the above-mentioned hot-dip plating and high-temperature austenitizing technology, wherein the sample 1-3 obtained in step 3 is immediately stamped and quickly cooled to room temperature after completing austenitization, thereby obtaining the zinc-aluminum-magnesium coated steel plate based on the hot-dip plating and high-temperature forming technology.

[0030] Furthermore, in the above technical solution, in step (1), the steel to be treated is heated into molten iron, and then subjected to molten iron pretreatment, converter smelting, off-furnace refining, and continuous casting to obtain a steel billet. Then, the steel billet is heated, rolled, controlled cooling, coiled, pickled, and cold rolled to obtain a steel plate. Finally, the steel plate is continuously annealed at an annealing temperature of 800±5°C and a dew point of -50±10°C to obtain a steel plate to be hot-dip coated.

[0031] The present invention provides an application of the zinc-aluminum-magnesium coated steel sheet based on hot-dip coating technology as a corrosion-resistant material. In a 3.5wt.% NaCl solution at 25°C, the corrosion current density I corr =(1.20-1.68)×10 -5 A / cm 2 .

[0032] The present invention provides an application of the zinc-aluminum-magnesium coated steel plate to be stamped based on the hot-dip coating and high-temperature austenitization technology as a high-temperature mechanical material, wherein the elongation after being kept at 920° C. for 1-3 minutes is 38-54%.

[0033] The technical effects of the present invention are as follows after experimental detection:

[0034] Cross-sectional SEM and EDS analysis of the hot-dip zinc-aluminum-magnesium coated steel sheet revealed that the coating contained a Zn-Al two-phase eutectic and a Zn-Al-MgZn2 three-phase eutectic. The combined eutectic content of the Zn-Al two-phase eutectic and the Zn-Al-MgZn2 three-phase eutectic was 50-95%. The Zn element existed as Zn and MgZn2 phases, with an interlamellar spacing of less than 1 micron. The intermediate compound layer between the steel sheet and the coating consisted of Fe-Al or Fe-Al-Zn intermetallic compounds, with a thickness of 0.3-3 microns.

[0035] The corrosion resistance test of the zinc-aluminum-magnesium coated steel sheet based on the hot-dip coating technology shows that the corrosion current density (I corr ) is (1.20-1.68)×10 -5 A / cm 2 .

[0036] The cross-sectional SEM and EDS tests of the zinc-aluminum-magnesium coated steel plate to be stamped based on the hot-dip coating and high-temperature austenitizing technology mentioned above show that the coating contains α-Fe(Zn,Al), and the Fe, Zn, Al, and Mg elements are evenly distributed in the α-Fe(Zn,Al) single layer structure.

[0037] The high temperature tensile mechanical property test of the zinc-aluminum-magnesium coated steel plate to be stamped based on the hot dip coating and high temperature austenitizing technology shows that the elongation is 38-54% under the conditions of a temperature of 920°C and a holding time of 1-3 minutes.

[0038] Therefore, the above experimental tests show that the present invention has the following advantages:

[0039] 1. The zinc-aluminum-magnesium coated steel sheet to be stamped, based on hot-dip plating and high-temperature austenitization technology, exhibits higher high-temperature tensile mechanical properties than the prior art. Specifically, at a temperature of 920°C and a holding time of 1-3 minutes, the sheet exhibits a tensile strength of 77.2 MPa and an elongation of 46.6%. Compared to the sheet coated with pure zinc in Reference Example 1, the elongation increases by 7.4% at the same temperature and holding time.

[0040] 2. The zinc-aluminum-magnesium coated steel sheet based on hot-dip coating technology of the present invention has higher corrosion resistance than the prior art, that is, in a 3.5wt.% NaCl solution at 25°C, the corrosion current density (I corr ) is 1.35×10 -5 A / cm 2 Compared with the plate with pure zinc in the immersion bath in Reference Example 1, the corrosion current density was reduced by 0.5×10 -5 A / cm 2 .

[0041] 3. The zinc-aluminum-magnesium coated steel plate to be stamped designed and prepared by the present invention based on hot-dip plating and high-temperature austenitization technology does not use rare earth elements, which reduces the raw material cost compared to the existing rare earth coating technology and is easy to commercialize and promote. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 shows the distribution of the plating solution components in the Zn-Al-Mg alloy liquid phase projection diagram calculated by the present invention, wherein Figure 1a shows the distribution position of the Zn-4.5Al-3.0Mg alloy in Example 1 and Reference Example 2 in the phase diagram; Figure 1b shows the distribution position of pure Zn in Reference Example 1 in the phase diagram; Figure 1c shows the distribution position of the Zn-4.5Al-1.1Mg alloy in Example 2 in the phase diagram; Figure 1d shows the distribution position of the Zn-6.0Al-3.6Mg alloy in Example 3 in the phase diagram; and Figure 1e shows the distribution position of the Zn-8.5Al-4.2Mg alloy in Example 4 in the phase diagram;

[0043] Figure 2 is a cross-sectional SEM image of samples 1-2, 0-2, 2-2, 3-2, and 4-2 prepared in Example 1, Reference Example 2, Reference Example 1, and Example 2-4 of the present invention;

[0044] Figure 3 is a potentiodynamic polarization curve image of samples 1-2, 0-2, 2-2, 3-2, and 4-2 prepared in Example 1, Reference Example 2, Reference Example 1, and Example 2-4 of the present invention in a 3.5 wt.% NaCl solution at 25°C;

[0045] Figure 4 is a cross-sectional SEM image of samples 1-3, 0-3, 0-3', 2-3, 3-3, and 4-3 obtained in Example 1, Reference Example 1-2, and Example 2-4 of the present invention;

[0046] Figure 5 is a stress-strain curve image of samples 1-3, 0-3, 2-3, 3-3, and 4-3 prepared in Example 1, Reference Example 1, and Examples 2-4 of the present invention at a temperature of 920°C and a holding time of 1-3 min. DETAILED DESCRIPTION

[0047] The present invention is further described in detail through embodiments and in conjunction with the accompanying drawings, but the present invention is not limited thereto.

[0048] By experimentally measuring the primary phases and phase contents of alloys with different compositions, a liquid phase projection surface diagram of the Zn-Al-Mg system was constructed. The phase equilibrium relationship of the Zn-Al-Mg system was established based on the phase composition. In this invention, some relevant data from the Zn-Al-Mg system liquid phase projection surface phase diagram database was disclosed to obtain the phase types and volume fractions in the Zn-Al-Mg alloy.

[0049] Based on the constructed Zn-Al-Mg system thermodynamic phase diagram database, thermodynamic calculations were used to obtain the corresponding alloys of Examples 1-4 and Reference Examples 1-2 as shown in FIG1 . The results are shown in Table 1.

[0050] Table 1 Zn-Al-Mg coating alloy composition

[0051] For ease of description, the sample naming principles in the examples of the present invention are explained below. The specific naming principle is: Sample ab, where a represents the serial number of the example and b represents the product of a specific step in each example. If the product is obtained from step 2 of example 1, it is named: Sample 1-2; if the product is obtained from step 3 of example 2, it is named: Sample 2-3.

[0052] Example 1:

[0053] A method for preparing a zinc-aluminum-magnesium coated steel sheet to be stamped based on hot-dip plating and high-temperature austenitizing technology, i.e., a zinc-aluminum-magnesium coated steel sheet having a plating solution composition of Zn-4.5Al-3.0Mg, specifically comprising the following steps:

[0054] Step 1, preparation of the steel sheet to be hot-dip coated, heating the steel material to be treated into molten iron, and then performing molten iron pretreatment, converter smelting, refining outside the furnace, and continuous casting to obtain a steel billet, then heating, rolling, controlled cooling, coiling, pickling, and cold rolling to obtain a steel sheet, and finally, continuously annealing the steel sheet at an annealing temperature of 800±5°C and a dew point of -50±10°C to obtain a steel sheet to be hot-dip coated;

[0055] To confirm the composition of the steel sheet to be hot-dip coated, an ICP test was conducted. The test results showed the following composition by weight: C: 0.33 wt.%, Si: 0.10 wt.%, Mn: 1.45 wt.%, P: no more than 0.020 wt.%, S: no more than 0.004 wt.%, Al: 0.080 wt.%, Ti: 0.02 wt.%, V: 0.18 wt.%, N: no more than 0.0040 wt.%, B: 0.0020 wt.%, and the remainder being Fe and unavoidable impurities.

[0056] Step 2: Hot-dip coating of the steel sheet to be hot-dip coated. First, a coating solution is prepared with the following mass percentages: Al content of 4.5 wt.%, Mg content of 3.0 wt.%, and the remainder being Zn and unavoidable impurities. Then, the steel sheet to be hot-dip coated obtained in step 1 is hot-dip coated at a coating temperature of 440-460° C., a coating time of 3-10 seconds, and a cooling rate of more than 30° C. / s to room temperature after the coating is completed. Thus, a zinc-aluminum-magnesium coated steel sheet based on the hot-dip coating technology is obtained, which is named Sample 1-2.

[0057] In order to verify the phase type and microstructure of the zinc-aluminum-magnesium coating in sample 1-2 obtained in step 2, SEM and EDS tests were performed on the cross section of sample 1-2. The test results are shown in Figure 2. Sample 1-2 consists of a steel plate, a zinc-aluminum-magnesium coating-2, and an intermediate compound layer between the steel plate and the coating;

[0058] The zinc-aluminum-magnesium coating-2 is composed of a Zn-Al two-phase eutectic and a Zn-Al-MgZn2 three-phase eutectic. The total eutectic content of the Zn-Al two-phase eutectic and the Zn-Al-MgZn2 three-phase eutectic is 95%. The Zn element exists in the form of Zn phase and MgZn2 phase, and the interlamellar spacing of the structure is less than 1 micron.

[0059] The intermediate compound layer is a Fe-Al or Fe-Al-Zn intermetallic compound with a thickness of 0.3-1 micron.

[0060] The test results show that the coating of sample 1-2 has a uniform structure and no local zinc enrichment.

[0061] In order to prove the corrosion resistance of sample 1-2, a corrosion resistance test was conducted. The test results are shown in Figure 3. In a 3.5 wt.% NaCl solution at 25°C, the corrosion current density (I corr ) is 1.35×10 -5 A / cm 2 The test results show that the Zn-Al-MgZn2 three-phase eutectic generated by hot-dip plating in step 2 can improve the corrosion resistance of zinc-aluminum-magnesium coated steel sheets.

[0062] Step 3, preparation of a zinc-aluminum-magnesium coated steel sheet to be stamped based on hot-dip coating and high-temperature austenitizing technology, austenitizing sample 1-2 obtained in step 2 at an austenitizing temperature of 920° C. and a holding time of 3 minutes, thereby obtaining a zinc-aluminum-magnesium coated steel sheet to be stamped based on hot-dip coating and high-temperature austenitizing technology, named sample 1-3;

[0063] To verify the phase composition and microstructure of the Zn-Al-Mg coating in Sample 1-3 obtained in Step 3, cross-sections of Sample 1-3 were subjected to SEM and EDS analysis. The test results, shown in Figure 4, show that Sample 1-3 consists of a steel plate and Zn-Al-Mg coating-3. The intermediate compound layer between the steel plate and Zn-Al-Mg coating-2 disappears. Zn-Al-Mg coating-3 consists of an α-Fe(Zn,Al) monolayer with uniform distribution of Fe, Zn, Al, and Mg. The Zn content ranges from 4.6-8.1 wt.%, Al from 0.7-1.2 wt.%, Mg from 0-0.1 wt.%, and O from 0.9-8.2 wt.%. These test results demonstrate that the austenitization in Step 3 transforms the coating structure from a Zn-Al two-phase eutectic and a Zn-Al-MgZn2 three-phase eutectic to an α-Fe(Zn,Al).

[0064] To demonstrate the mechanical properties of samples 1-3 under high-temperature conditions, high-temperature tensile testing was conducted. The test results, shown in Figure 5, show that at 920°C and a holding time of 3 minutes, the tensile strength of samples 1-3 was 77.2 MPa and the elongation was 46.6%. These test results demonstrate that the austenitization step (step 3) improves the high-temperature mechanical properties of the zinc-aluminum-magnesium coated steel sheets to be stamped, using a hot-dip coating and high-temperature austenitization process.

[0065] Step 4, stamping and forming the zinc-aluminum-magnesium coated steel plate to be stamped based on hot-dip plating and high-temperature austenitizing technology. After the sample 1-3 obtained in step 3 is austenitized, it is immediately stamped and quickly cooled to room temperature to obtain the zinc-aluminum-magnesium coated steel plate based on hot-dip plating and high-temperature forming technology.

[0066] In order to demonstrate the influence of Al and Mg elements in the plating solution on the performance of the plated plate, reference example 1 is provided, in which the plating solution is a pure zinc plated plate, that is, the plating solution does not contain aluminum or magnesium elements.

[0067] Reference Example 1

[0068] A coating plate whose immersion bath is pure zinc, wherein the steps not otherwise specified are the same as those in Example 1, except that: the immersion bath in step 2 is pure zinc, without the addition of Al and Mg elements; the product obtained in step 2 is named sample 0-2, and the product obtained in step 3 is named sample 0-3.

[0069] The SEM and EDS test results of sample 0-2 are shown in Figure 2. Sample 0-2 consists of a steel plate, a coating, and an intermediate compound layer between the steel plate and the coating.

[0070] The coating consists of pure Zn phase;

[0071] The intermediate compound layer is a Fe-Zn intermetallic compound with a thickness of 10 microns. There are many microcracks in the intermediate compound layer.

[0072] The test results show that due to the lack of aluminum and magnesium elements added to the immersion plating solution, there is no eutectic structure in the coating of sample 0-2. Compared with Example 1, Example 1 obtains Zn-Al two-phase eutectic and Zn-Al-MgZn2 three-phase eutectic through its immersion plating solution.

[0073] The corrosion resistance test results of sample 0-2 are shown in FIG3 . In a 3.5 wt. % NaCl solution at 25° C., the corrosion current density (I corr ) is 1.85×10 -5 A / cm 2 The test results show that the Zn-Al two-phase eutectic and Zn-Al-MgZn2 three-phase eutectic obtained by the immersion plating solution of Example 1 improve its corrosion resistance.

[0074] The SEM and EDS test results of sample 0-3 are shown in Figure 4. In sample 0-3, the intermediate compound layer between the steel plate and the coating disappears, and the sample is composed of the steel plate and the coating. Among them, the coating is composed of an α-Fe(Zn) single layer structure, and the Zn element in the α-Fe(Zn) single layer structure is enriched at the contact point with the steel plate.

[0075] The test results show that the coating structure is transformed from pure Zn phase to α-Fe(Zn) through austenitization in step 3. Compared with Example 1, liquid zinc comes into contact with the steel sheet during the austenitization process.

[0076] The high-temperature tensile mechanical properties test results of Samples 0-3 are shown in Figure 5. After holding at 920°C for 3 minutes, the tensile strength was 86.9 MPa, and the elongation was 39.2%. These test results demonstrate that, compared to Example 1, the liquid zinc in Example 1 did not come into contact with the steel sheet during the austenitization process, resulting in a higher elongation of the coated sheet.

[0077] In order to demonstrate the effect of austenitizing temperature on the microscopic distribution uniformity of coating components, a reference example 2 is provided. The immersion bath is the Zn-4.5Al-3.0Mg coating plate in Example 1, but its austenitizing temperature is 850°C.

[0078] Reference Example 2

[0079] A plated plate with a Zn-4.5Al-3.0Mg plating solution, wherein the steps not otherwise specified are the same as those in Example 1, except that: the product obtained in step 2 is named sample 0-2'; the austenitizing temperature in step 3 is 850°C, and the product obtained in step 3 is named sample 0-3'.

[0080] The results and conclusions of the SEM test, EDS test, and corrosion resistance test of sample 0-2' are the same as those of Example 1.

[0081] The SEM and EDS test results of sample 0-3' are shown in Figure 4. In sample 0-3', the thin intermediate compound layer between the steel plate and the coating disappears, and the sample is composed of the steel plate and the coating. The lower layer of the coating is composed of an α-Fe(Zn) single layer structure, and the Zn element in the α-Fe(Zn) single layer structure is enriched at the contact point with the steel plate. The upper layer of the coating is composed of an α-Fe(Zn,Al) single layer structure, and there is enrichment of Zn and Al elements.

[0082] The test results show that after austenitization in step 3, the coating structure is stratified, with the Zn-Al-MgZn2 three-phase eutectic transforming into a lower layer of α-Fe(Zn) and an upper layer of α-Fe(Zn,Al). Compared with Example 1, the coating structure becomes uneven during the austenitization process.

[0083] In order to demonstrate the influence of the eutectic structure in the coating on the performance of the coated plate, that is, to simultaneously demonstrate the effect of the thermodynamic phase diagram of the Zn-Al-Mg system on the technical solution, Examples 2, 3 and 4 are provided.

[0084] The composition of the plating solution of Example 2 is determined based on the Zn-Al two-phase eutectic line in the phase diagram. The specific mass percentages of the plating solution components are: Zn content is 94.4wt.%, Al content is 4.5wt.%, Mg content is 1.1wt.%, and the plating solution is referred to as plating solution A.

[0085] The composition of the plating solution of Example 3 is determined based on the Al-MgZn2 two-phase eutectic line in the phase diagram. The specific mass percentages of the plating solution components are: Zn content is 90.4wt.%, Al content is 6.0wt.%, Mg content is 3.6wt.%, and the plating solution is referred to as plating solution B.

[0086] The composition of the plating solution of Example 4 is determined based on the Al-MgZn2 two-phase eutectic line in the phase diagram. The specific mass percentages of the plating solution components are: Zn content is 87.3wt.%, Al content is 8.5wt.%, Mg content is 4.2wt.%, and the plating solution is referred to as plating solution C.

[0087] Example 2

[0088] A zinc-aluminum-magnesium coated steel plate whose immersion bath is bath A, wherein the steps not otherwise specified are the same as those in Example 1, except that: the immersion bath in step 2 is bath A; the product obtained in step 2 is named sample 2-2, and the product obtained in step 3 is named sample 2-3.

[0089] The SEM and EDS test results of sample 2-2 are shown in Figure 2. Sample 2-2 consists of a steel plate, a coating, and an intermediate compound layer between the steel plate and the coating; wherein the coating consists of a pure Zn phase and a Zn-Al two-phase eutectic, and the Zn-Al two-phase eutectic content is 50%; the intermediate compound layer is an Fe-Al or Fe-Al-Zn intermetallic compound with a thickness of 0.3-1 micron.

[0090] The test results show that due to the change in the composition of the immersion solution, the content of Zn-Al two-phase eutectic structure in the coating of sample 2-2 is higher. Compared with Example 1, Example 2 contains more Zn-Al two-phase eutectic.

[0091] The corrosion resistance test results of sample 2-2 are shown in FIG3 . In a 3.5 wt.% NaCl solution at 25°C, the corrosion current density (I corr ) is 1.20×10 -5 A / cm 2 The test results show that due to the change in the composition of the immersion bath, Example 2 contains more Zn-Al two-phase eutectic, which enables it to obtain higher corrosion resistance.

[0092] The SEM and EDS test results of sample 2-3 are shown in Figure 4. In sample 2-3, the intermediate compound layer between the steel plate and the coating disappears, and the sample is composed of the steel plate and the coating; wherein the coating is composed of an α-Fe(Zn,Al) single-layer structure, and the Fe, Zn, and Al elements are evenly distributed in the α-Fe(Zn,Al) single-layer structure, with a Zn content of 3.5-7.5wt.%, an Al content of 0.5-1.7wt.%, Mg of 0-0.1wt.%, and O of 0.5-10.0wt.%.

[0093] The test results show that through the austenitization in step 3, the coating structure is transformed from pure Zn phase and Zn-Al two-phase eutectic to α-Fe(Zn,Al), and its structure is similar to that of Example 1.

[0094] The high-temperature tensile mechanical properties test results of Sample 2-3 are shown in Figure 5. The tensile strength after holding at 900°C for 1 minute is 75.8 MPa and the elongation is 46.0%. The test results show that the elongation is reduced by austenitization in step 3.

[0095] By comparing Example 1 and Example 2, it can be seen that the increase in the Zn-Al two-phase eutectic content improves the corrosion resistance, but reduces the elongation.

[0096] Example 3

[0097] A zinc-aluminum-magnesium coated steel plate whose immersion bath is bath B, the steps not otherwise specified are the same as those in Example 1, except that: the immersion bath in step 2 is bath B; the product obtained in step 2 is named sample 3-2, and the product obtained in step 3 is named sample 3-3.

[0098] The SEM test and EDS test results of sample 3-2 are shown in Figure 2. Sample 3-2 consists of a steel plate, a coating, and an intermediate compound layer between the steel plate and the coating; wherein the coating is composed of Zn-Al two-phase eutectic and Al-MgZn2 two-phase eutectic, the Al-MgZn2 two-phase eutectic content is 80%, the interlamellar spacing of the Al-MgZn2 two-phase eutectic structure is less than 1 micron, and the Zn element in the Al-MgZn2 two-phase eutectic exists in the form of MgZn2; the intermediate compound layer is a Fe-Al or Fe-Al-Zn intermetallic compound with a thickness of 1-2 microns.

[0099] The test results show that due to the change in the composition of the immersion solution, the content of Al-MgZn2 two-phase eutectic structure in the coating of sample 3-2 is higher. Compared with Example 1, Example 3 contains more Al-MgZn2 two-phase eutectic.

[0100] The corrosion resistance test results of sample 3-2 are shown in FIG3 . In a 3.5 wt.% NaCl solution at 25°C, the corrosion current density (I corr ) is 1.52×10 -5 A / cm 2 The test results show that due to the change in the composition of the immersion bath, Example 3 contains more Al-MgZn2 two-phase eutectic, which reduces its corrosion resistance.

[0101] The SEM test and EDS test results of sample 3-3 are shown in Figure 4. In sample 3-3, the intermediate compound layer between the steel plate and the coating disappears, and the sample is composed of the steel plate and the coating; wherein the coating is composed of an α-Fe(Zn,Al) single-layer structure, and the Fe, Zn, and Al elements are evenly distributed in the α-Fe(Zn,Al) single-layer structure, with a Zn content of 7.2-10.3wt.%, an Al content of 7.8-12.2wt.%, Mg of 0-0.2wt.%, and O of 0.9-5.6wt.%.

[0102] The test results show that through the austenitization in step 3, the coating structure is transformed from Zn-Al two-phase eutectic and Al-MgZn2 two-phase eutectic to α-Fe(Zn,Al), and its organizational structure is similar to that of Example 1.

[0103] The high-temperature tensile mechanical properties test results of Sample 3-3 are shown in Figure 5. The tensile strength after holding at 900°C for 3 minutes is 77.1 MPa, and the elongation is 53.2%. The test results show that the elongation is improved compared to Example 1 through austenitization in Step 3.

[0104] By comparing Example 1 and Example 3, it can be seen that the increase in the Al-MgZn2 two-phase eutectic content reduces the corrosion resistance but improves the elongation.

[0105] Example 4

[0106] A zinc-aluminum-magnesium coated steel plate whose immersion bath is bath C, wherein the steps not otherwise specified are the same as those in Example 1, except that: the immersion bath in step 2 is bath C; the product obtained in step 2 is named sample 4-2, and the product obtained in step 3 is named sample 4-3.

[0107] The SEM test and EDS test results of sample 4-2 are shown in Figure 2. Sample 4-2 consists of a steel plate, a coating, and an intermediate compound layer between the steel plate and the coating; wherein the coating is composed of Zn-Al two-phase eutectic and Al-MgZn2 two-phase eutectic, the Al-MgZn2 two-phase eutectic content is 80%, the interlamellar spacing of the Al-MgZn2 two-phase eutectic structure is less than 1 micron, and the Zn element in the Al-MgZn2 two-phase eutectic exists in the form of MgZn2; the intermediate compound layer is a Fe-Al or Fe-Al-Zn intermetallic compound with a thickness of 2-3 microns.

[0108] The test results show that compared with Example 1, the microstructure uniformity in the coating is poor.

[0109] The corrosion resistance test results of sample 4-2 are shown in FIG3 . In a 3.5 wt. % NaCl solution at 25° C., the corrosion current density (I corr ) is 1.68×10 -5 A / cm 2 The test results show that due to the change in the composition of the immersion bath, Example 4 contains more Al-MgZn2 two-phase eutectic, which reduces its corrosion resistance.

[0110] The SEM and EDS test results of sample 4-3 are shown in Figure 4. In sample 4-3, the intermediate compound layer between the steel plate and the coating disappears, and the sample is composed of the steel plate and the coating. Among them, the coating is composed of an α-Fe(Zn,Al) single layer structure, and the Zn element in the α-Fe(Zn,Al) single layer structure is enriched at the contact point with the steel plate.

[0111] The test results show that through the austenitization in step 3, the coating structure is transformed from Zn-Al two-phase eutectic and Al-MgZn2 two-phase eutectic to α-Fe(Zn,Al). Compared with Example 1, liquid zinc comes into contact with the steel plate during the austenitization process.

[0112] The high-temperature tensile mechanical properties test results of Sample 4-3 are shown in Figure 5. The tensile strength after holding at 920°C for 1 minute is 82.6 MPa, and the elongation is 38.0%. The test results show that the elongation is significantly reduced compared to Example 1 due to the austenitization in Step 3.

[0113] By comparing and analyzing Examples 1-4 and Reference Examples 1-2, the following conclusions can be drawn:

[0114] 1. The corrosion resistance of zinc-aluminum-magnesium coated steel sheets based on hot-dip coating technology increases with the increase of the content of Zn-Al two-phase eutectic in the coating structure, and decreases with the increase of the content of Al-MgZn2 two-phase eutectic;

[0115] 2. The elongation of the zinc-aluminum-magnesium coated steel sheet to be stamped based on hot-dip coating and high-temperature austenitization technology decreases with the increase of the content of Zn-Al two-phase eutectic in the coating structure, and increases with the increase of the content of Al-MgZn2 two-phase eutectic;

[0116] Therefore, according to the above analysis, it can be seen that the present invention can achieve significant technical effect improvement by calculating the phase diagram and adopting the method of preparing zinc-aluminum-magnesium coated steel plate by austenitization.

[0117] In summary, the above embodiment of the present invention prepares a method for preparing a zinc-aluminum-magnesium coated steel sheet to be stamped based on hot-dip plating and high-temperature austenitizing technology, uses phase diagram calculation to guide component design, prepares materials according to the mass percentage of the plating solution components: Zn content of 85-95wt.%, Al content of 4.5-8.5wt.%, and Mg content of 1-4.5wt.%, and obtains a zinc-aluminum-magnesium coated steel sheet based on hot-dip plating and high-temperature forming technology after hot-dip plating. The zinc-aluminum-magnesium coated steel sheet prepared by the present invention forms a Zn-Al-MgZn2 three-phase eutectic in the coating structure after hot-dip plating. When the Zn element content is 92.5wt.%, the Al element content is 4.5wt.%, and the Mg element content is 3.0wt.%, the corrosion current density (Icorr ) is 1.35×10 -5 A / cm 2 At the same time, under the conditions of 900-920℃ and keeping warm for 1-3 minutes, the elongation is 46.6%.

Claims

1. A zinc-aluminum-magnesium coated steel sheet to be stamped based on hot-dip coating and high-temperature austenitizing technology, characterized in that: The steel plate is obtained by hot-dip galvanizing and austenitizing under high temperature conditions; The hot-dip plating solution is a Zn-Al-Mg plating solution, and the specific mass percentage of the Zn-Al-Mg plating solution is: Al content is 4.5-8.5wt.%, Mg content is 1-4.5wt.%, and the rest is Zn and unavoidable impurities; The steel plate becomes a zinc-aluminum-magnesium coated steel plate based on hot-dip coating technology after hot-dip coating. The zinc-aluminum-magnesium coated steel plate based on hot-dip coating technology is composed of a steel plate, a zinc-aluminum-magnesium coating layer-2, and an intermediate compound layer between the steel plate and the coating layer, wherein: The zinc-aluminum-magnesium coating-2 comprises Zn, Al, and MgZn2 phases; the zinc-aluminum-magnesium coating-2 comprises Zn-Al two-phase eutectic and Zn-Al-MgZn2 three-phase eutectic, the total eutectic content of the Zn-Al two-phase eutectic and the Zn-Al-MgZn2 three-phase eutectic is 50-95%, and the interlamellar spacing of the eutectic structure is less than 1 micron; The intermediate compound layer between the steel plate and the coating, referred to as the intermediate compound layer, is a Fe-Al or Fe-Al-Zn intermetallic compound; The zinc-aluminum-magnesium coated steel sheet based on the hot-dip coating technology is austenitized at 900-920° C. to become a zinc-aluminum-magnesium coated steel sheet to be stamped based on the hot-dip coating and high-temperature austenitization technology; The zinc-aluminum-magnesium coated steel plate to be stamped based on hot-dip plating and high-temperature austenitizing technology is composed of a steel plate and a zinc-aluminum-magnesium coating-3, and the zinc-aluminum-magnesium coating-3 is composed of an α-Fe (Zn, Al) single-layer structure, and the Fe, Zn, Al, and Mg elements are evenly distributed in the α-Fe (Zn, Al) single-layer structure, and the Zn element content is 3.5-10.3wt.%, the Al element content is 0.5-12.2wt.%, Mg is 0-0.2wt.%, and O is 0.5-8.2wt.%.

2. The zinc-aluminum-magnesium coated steel sheet to be stamped based on hot-dip coating and high-temperature austenitizing technology according to claim 1, characterized in that: The mass percentages of the steel plate components are: C content is 0.31-0.35wt.%, Si content is 0.05-0.20wt.%, Mn content is 1.40-1.50wt.%, P content is not more than 0.020wt.%, S content is not more than 0.004wt.%, Al content is not less than 0.060wt.%, Ti content is 0.010-0.025wt.%, V content is 0.16-0.20wt.%, N content is not more than 0.0045wt.%, B content is 0.0010-0.0030wt.%, and the rest is Fe and unavoidable impurities.

3. The zinc-aluminum-magnesium coated steel sheet to be stamped based on hot-dip coating and high-temperature austenitizing technology according to claim 1, characterized in that: In the Zn-Al two-phase eutectic and the Zn-Al-MgZn2 three-phase eutectic of the zinc-aluminum-magnesium coating-2, the Zn element exists in the form of Zn phase and MgZn2 phase, and the Al element exists in the form of Al phase; The interlamellar spacing of the eutectic structure is less than 1 micron.

4. The zinc-aluminum-magnesium coated steel sheet to be stamped based on hot-dip coating and high-temperature austenitizing technology according to claim 1, characterized in that: The thickness of the intermediate compound layer is 0.3-3 microns.

5. The zinc-aluminum-magnesium coated steel sheet based on hot-dip coating and high-temperature austenitizing technology according to claim 1, characterized in that: The Zn content in the immersion plating solution is 85-95wt.%.

6. A method for preparing a zinc-aluminum-magnesium coated steel sheet to be stamped based on hot-dip coating and high-temperature austenitizing technology, characterized in that The following steps are involved: Step 1, preparation of a steel plate to be hot dipped; Step 2, hot-dip plating of the steel sheet to be hot-dip plated, first preparing a plating solution, and then hot-dip plating the steel sheet to be hot-dip plated obtained in step 1, that is, obtaining a zinc-aluminum-magnesium coated steel sheet based on hot-dip plating technology, named sample 1-2; Step 3, austenitizing the zinc-aluminum-magnesium coated steel sheet based on hot-dip coating technology, austenitizing the sample 1-2 obtained in step 2, that is, obtaining the zinc-aluminum-magnesium coated steel sheet to be stamped based on hot-dip coating and high-temperature austenitizing technology, named sample 1-3.

7. The preparation method according to claim 6, characterized in that: In the step 1, the steel material to be processed is heated into molten iron, and then subjected to molten iron pretreatment, converter smelting, refining outside the furnace, and continuous casting to obtain a steel billet. Then, the steel billet is heated, rolled, controlled cooling, coiled, pickled, and cold rolled to obtain a steel plate. Finally, the steel plate is continuously annealed at an annealing temperature of 800±5°C and a dew point of -50±10°C to obtain a steel plate to be hot-dip plated. In step 2, the mass percentage of the immersion plating solution is: Al content is 4.5-8.5wt.%, Mg content is 1-4.5wt.%, and the rest is Zn and unavoidable impurities; In step 2, the hot dip coating conditions are as follows: the coating temperature is 440-460° C., the coating time is 3-10 seconds, and the cooling rate after the coating is completed is greater than 30° C. / s to cool to room temperature.

8. The preparation method according to claim 6, characterized in that: In the step 3, the austenitizing conditions are: the austenitizing temperature is 900-920° C., and the holding time is 1-3 min.

9. Application of the zinc-aluminum-magnesium coated steel sheet to be stamped based on hot-dip coating and high-temperature austenitizing technology as claimed in any one of claims 1 to 5 as a high-temperature mechanical material.

Citation Information

Patent Citations

  • Ultra-high strength zinc-aluminum-magnesium coated steel sheet for high-temperature forming and its manufacturing method

    CN107099748B

  • 1250MPa Grade ultrahigh-strength zinc-aluminum-magnesium coated steel plate and production method thereof

    CN104419867A

  • Super-strength zinc aluminum magnesium coated steel plate for high-temperature shaping and manufacture method thereof

    CN107099748A

  • Hot dip zn alloy plated steel sheet having excellent Anti-corrosion and method for manufacturing the steel sheet using the same

    KR1020150052376A

  • Hot dip zn-based alloy coating bath comprising calcium oxide, hot dip zn-based alloy coated steel sheet and method for preparing the same

    KR1020150073314A