Cemented carbide matrix, and polycrystalline diamond compact and preparation method therefor

By introducing specific metal additives into the cemented carbide matrix of polycrystalline diamond composite sheets to form an anti-corrosion bonding phase, the problem of poor corrosion resistance of the cemented carbide matrix is ​​solved, and the corrosion resistance and corrosion resistance of polycrystalline diamond composite sheets are significantly improved. Erosion resistance extends service life.

WO2024212442A1PCT designated stage expired Publication Date: 2024-10-17SHENZHEN HAIMINGRUN SUPERHARD MATERIALS
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/119506
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-14
Filing Date
2023-09-18
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

The carbide matrix of existing polycrystalline diamond composite sheets has poor corrosion resistance, resulting in reduced performance and service life, and is prone to early failure especially during drilling.

Method used

Introducing cobalt and other metal additives, such as nickel, chromium, manganese, molybdenum, tin, copper, palladium, silver, aluminum, and platinum, into the cemented carbide matrix to form an anti-corrosion bonding phase, and control its mass ratio to improve corrosion resistance properties, and prepare polycrystalline diamond composite sheets through sintering.

Benefits of technology

It effectively improves the corrosion resistance and erosion resistance of polycrystalline diamond composite sheets, extends the service life, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023119506_17102024_PF_FP_ABST
    Figure CN2023119506_17102024_PF_FP_ABST
Patent Text Reader

Abstract

A cemented carbide matrix, and a polycrystalline diamond compact and a preparation method therefor. The cemented carbide matrix comprises a binding phase and tungsten carbide; the binding phase comprises cobalt and a metal additive; and the metal additive is selected from one or more of nickel, chromium, manganese, molybdenum, tin, copper, palladium, silver, aluminum, and platinum. A corrosion-resistant binding phase is formed by introducing specific elements and controlling the proportion thereof, so as to improve the corrosion resistance of the cemented carbide matrix. The corrosion-resistant binding phase changes the corrosion mechanism of the cemented carbide matrix, and the corrosion mechanism is more suitable for a usage scenario of the polycrystalline diamond compact, so that the corrosion resistance and the erosion resistance of the polycrystalline diamond compact are effectively improved, thereby prolonging the service life of the compact.
Need to check novelty before this filing date? Find Prior Art

Description

A cemented carbide substrate, polycrystalline diamond composite sheet and preparation method thereof Technical Field

[0001] The present invention relates to the technical field of superhard materials, and in particular to a cemented carbide substrate, a polycrystalline diamond composite sheet and a preparation method thereof. Background Art

[0002] Polycrystalline Diamond Compacts (PDCs) are ultra-hard composite materials composed of polycrystalline diamond layers and cemented carbide layers. Due to their exceptional wear resistance of the diamond layer and the impact toughness of the cemented carbide, they are widely used in geological and oil drilling. During drilling operations, geological environments vary significantly from region to region, with varying geological composition at varying depths. Furthermore, the drilling process itself induces localized high temperatures and material input, resulting in the PDCs facing a complex chemical environment during operation, creating a harsh, corrosive environment for metals.

[0003] During drilling, polycrystalline diamond compacts (PCDs) are mounted on a drill bit and rotate at high speed to cut rock layers. This process produces a mixture of rock chips, diamond chips, and mud, which erode the compacts. The carbide substrate in a PCD is the primary site of corrosion. This binder phase, composed of one or more transition metals, is more susceptible to corrosion than tungsten carbide, leading to structural defects in the carbide and affecting overall performance.

[0004] Currently, polycrystalline diamond composite sheets primarily use cobalt-based cemented carbide as the synthetic matrix. For WC-Co cemented carbide, galvanic corrosion easily forms between the binder and the carbide, promoting binder dissolution and damaging the integrity of the microstructure. Chemical corrosion and erosion can impair the mechanical properties of the cemented carbide and lead to premature failure. Due to the inherent brittleness of tungsten carbide, its strength is extremely sensitive to the presence of tiny defects. Localized damage caused by corrosion and erosion, especially in the initial stages, leads to a rapid loss of strength. This damage mechanism, combined with erosion during the drilling process, leads to the expansion of localized damage, reducing the performance and service life of the diamond composite sheet.

[0005] Therefore, the existing technology still needs to be improved and developed.

[0006] Summary of the Invention

[0007] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a cemented carbide substrate, a polycrystalline diamond composite sheet and a preparation method thereof, aiming to solve the problem that the existing cemented carbide substrate has poor corrosion resistance, which reduces the performance and service life of the diamond composite sheet.

[0008] The technical solutions of the present invention are as follows:

[0009] A cemented carbide substrate comprises a binder phase and tungsten carbide; the binder phase comprises cobalt and a metal additive; the metal additive is selected from one or more of nickel, chromium, manganese, molybdenum, tin, copper, palladium, silver, aluminum, and platinum.

[0010] The cemented carbide matrix, wherein the mass proportion of the binder phase in the cemented carbide matrix is ​​13%-20%.

[0011] The cemented carbide substrate, wherein the mass of cobalt in the binder phase accounts for 0.5%-16% of the cemented carbide substrate.

[0012] The cemented carbide substrate, wherein the mass of each metal additive in the binder phase accounts for 0.5%-16% of the cemented carbide substrate.

[0013] In the cemented carbide substrate, the mass of cobalt in the binder phase accounts for 5%-95%.

[0014] In the cemented carbide substrate, the total mass of the metal additives accounts for 5%-95% of the binder phase.

[0015] A polycrystalline diamond composite sheet comprises a polycrystalline diamond layer and a cemented carbide matrix.

[0016] A method for preparing a polycrystalline diamond compact comprises the following steps:

[0017] Mixing diamond formula powder to obtain mixed powder;

[0018] placing a cemented carbide substrate on the mixed powder to obtain an assembly block;

[0019] The assembly block is sintered to obtain a polycrystalline diamond compact.

[0020] The method for preparing the polycrystalline diamond composite sheet, wherein the temperature of the sintering treatment is 1400-2000° C., the pressure of the sintering treatment is 5-10 GPa, and the time of the sintering treatment is 5-60 minutes.

[0021] Beneficial effects: The present invention provides a cemented carbide substrate, a polycrystalline diamond composite sheet, and a preparation method thereof, wherein the cemented carbide substrate comprises a binding phase and tungsten carbide; the binding phase comprises cobalt and a metal additive; the metal additive is selected from one or more of nickel, chromium, manganese, molybdenum, tin, copper, palladium, silver, aluminum, and platinum. The present invention improves the corrosion resistance of the cemented carbide substrate by introducing specific elements and controlling their proportions to form a corrosion-resistant binding phase. Since the corrosion-resistant binding phase changes the corrosion mechanism of the cemented carbide substrate, the corrosion mechanism is more suitable for the use scenario of the polycrystalline diamond composite sheet, thereby effectively improving the corrosion resistance and erosion resistance of the polycrystalline diamond composite sheet, thereby increasing the service life of the composite sheet. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] FIG1 is a schematic diagram of the cross-sectional structure of a polycrystalline diamond compact of the present invention;

[0023] FIG2 is a comparison diagram of the weight loss of polycrystalline diamond compacts of Examples 1, 2, 3, and 4 of the present invention after oscillation erosion for 100 hours;

[0024] FIG3 is a comparison diagram of the weight loss of polycrystalline diamond compacts of Examples 1, 2, 3, and 4 of the present invention after constant temperature corrosion for 100 hours;

[0025] FIG4 is a comparative diagram of weight loss of polycrystalline diamond compacts according to Examples 1, 2, 3, and 4 of the present invention after constant temperature corrosion for 100 hours in a pH 4.0 environment. DETAILED DESCRIPTION

[0026] The present invention provides a cemented carbide substrate, a polycrystalline diamond compact, and a method for preparing the same. To clarify the objectives, technical solutions, and effects of the present invention, the present invention is described in further detail below. It should be understood that the specific embodiments described herein are intended only to illustrate the present invention and are not intended to limit the present invention.

[0027] It will be understood by those skilled in the art that, unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by those skilled in the art in the art to which the present invention belongs. It should also be understood that terms such as those defined in common dictionaries should be understood to have meanings consistent with their meanings in the context of the prior art and will not be interpreted in an idealized or overly formal sense unless specifically defined as herein.

[0028] The present invention provides a cemented carbide substrate, which comprises a binder phase and tungsten carbide; the binder phase comprises cobalt and a metal additive; the metal additive is selected from one or more of nickel, chromium, manganese, molybdenum, tin, copper, palladium, silver, aluminum, and platinum.

[0029] In this embodiment, the corrosion resistance of the cemented carbide matrix is ​​improved by introducing specific elements into the cemented carbide matrix and controlling their proportions to form a corrosion-resistant bonding phase; that is, one or more of nickel, chromium, manganese, molybdenum, tin, copper, palladium, silver, aluminum, platinum and cobalt are used as the bonding phase of the cemented carbide matrix to form a cemented carbide matrix with tungsten carbide, so that the bonding phase can change the corrosion mechanism of the cemented carbide matrix, so that the corrosion mechanism is more suitable for the use scenario of the polycrystalline diamond composite sheet, thereby effectively improving the corrosion resistance and erosion resistance of the polycrystalline diamond composite sheet, and then increasing the service life of the polycrystalline diamond composite sheet.

[0030] In some embodiments, the binder phase accounts for 13% to 20% by mass in the cemented carbide matrix. Controlling the binder phase mass in the cemented carbide matrix to be between 13% and 20% can improve the bonding strength between the raw materials of the cemented carbide matrix, thereby making the cemented carbide matrix have higher strength and less prone to cracking during use, while also improving the wear resistance of the cemented carbide matrix.

[0031] In some embodiments, the mass of cobalt in the binder phase is 0.5%-16% of the cemented carbide substrate. Cobalt plays a major catalytic role in the binder phase. Controlling the cobalt content in the cemented carbide substrate to between 0.5% and 16% can improve the bonding strength between tungsten carbides.

[0032] In some embodiments, the mass of each metal additive in the binder phase accounts for 0.5% to 16% of the cemented carbide substrate. Using one or more of nickel, chromium, manganese, molybdenum, tin, copper, palladium, silver, aluminum, and platinum as the metal additive in the binder phase, and controlling the mass of each metal additive to account for 0.5% to 16% of the cemented carbide substrate, can impart superior corrosion and erosion resistance to the cemented carbide substrate, thereby improving the corrosion resistance of the cemented carbide substrate and extending the service life of the polycrystalline diamond compact.

[0033] In some embodiments, the mass ratio of cobalt in the binder phase is 5%-95%. When the mass ratio of cobalt in the binder phase is within this range, it can play a better catalytic role.

[0034] In some embodiments, the total mass of the metal additives accounts for 5%-95% of the binder phase. When the total mass of the metal additives accounts for 5%-95% of the binder phase, the cemented carbide substrate can have better corrosion resistance.

[0035] In addition, as shown in FIG1 , the present invention further provides a polycrystalline diamond compact, comprising a polycrystalline diamond layer 1 and a cemented carbide substrate 2 .

[0036] In this embodiment, the polycrystalline diamond compact produced using the cemented carbide substrate and the polycrystalline diamond layer has a binder phase in the cemented carbide substrate that changes the corrosion mechanism of the cemented carbide substrate, making the corrosion mechanism more suitable for the use scenario of the polycrystalline diamond compact, thereby effectively improving the corrosion resistance and erosion resistance of the polycrystalline diamond compact, thereby increasing the service life of the polycrystalline diamond compact. Furthermore, using the cemented carbide substrate as the substrate of the polycrystalline diamond compact can make the polycrystalline diamond compact have higher corrosion resistance, while also making the polycrystalline diamond compact have better properties such as high hardness and wear resistance, thereby increasing the service life of the compact and reducing production costs.

[0037] At the same time, the present invention also provides a method for preparing a polycrystalline diamond compact, comprising the steps of:

[0038] Step S10: mixing the diamond formula powder to obtain mixed powder;

[0039] Step S20: placing a cemented carbide substrate on the mixed powder to obtain an assembly block;

[0040] Step S30: sintering the assembly block to obtain a polycrystalline diamond compact.

[0041] Specifically, the embodiment stacks the mixed powder and cemented carbide substrate in a metal cup and sinters them in high-temperature, high-pressure equipment to produce a polycrystalline diamond compact. The polycrystalline diamond compact has a substrate comprising the aforementioned cemented carbide substrate, which includes a binder phase and tungsten carbide; the binder phase includes cobalt and a metal additive; the metal additive is selected from one or more of nickel, chromium, manganese, molybdenum, tin, copper, palladium, silver, aluminum, and platinum. The binder phase modifies the corrosion mechanism of the cemented carbide substrate, thereby improving the corrosion and erosion resistance of the polycrystalline diamond compact.

[0042] Furthermore, the carbide matrix of the polycrystalline diamond composite sheet contains a corrosion-resistant bonding phase, which contains cobalt and at least one metal additive. The corrosion-resistant bonding phase changes the dominant corrosion mechanism, thereby making the carbide matrix corrosion-resistant.

[0043] Specifically, in step S20, the mixed powder is first introduced into a metal cup, flattened, and then the cemented carbide substrate is placed into the metal cup and positioned above the mixed powder to obtain an assembly block.

[0044] In some embodiments, the sintering temperature is 1400-2000°C, the sintering pressure is 5-10 GPa, and the sintering time is 5-60 minutes. Sintering the assembly block under these conditions can produce a polycrystalline diamond compact with good corrosion resistance, good impact resistance, and high wear resistance.

[0045] In some embodiments, step S30 further includes placing the assembly block in pyrophyllite and placing it in a high-pressure device for sintering to obtain a polycrystalline diamond compact blank; then processing the polycrystalline diamond compact blank to a target size to obtain a polycrystalline diamond compact.

[0046] The present invention will be described in detail with reference to the following examples. It should also be understood that the following examples are only intended to further illustrate the present invention and are not to be construed as limiting the scope of protection of the present invention. Any non-essential improvements and adjustments made by those skilled in the art based on the above disclosure of the present invention fall within the scope of protection of the present invention.

[0047] Example 1

[0048] This embodiment provides a polycrystalline diamond compact, comprising a polycrystalline diamond layer and a cemented carbide substrate. The cemented carbide substrate contains 14% by weight cobalt as a binder phase, with the remainder being tungsten carbide. The polycrystalline diamond layer and the cemented carbide substrate are sintered under hot-pressing conditions at 1400°C and 7.5 GPa for 10 minutes to produce the polycrystalline diamond compact.

[0049] Example 2

[0050] This embodiment provides a polycrystalline diamond compact, comprising a polycrystalline diamond layer and a cemented carbide substrate. The cemented carbide substrate comprises a 14%wt binder phase comprising 7wt% cobalt and 7wt% nickel, with the remainder being tungsten carbide. The polycrystalline diamond layer and the cemented carbide substrate are sintered under hot-pressing conditions at 1400°C and 7.5 GPa for 10 minutes to produce the polycrystalline diamond compact.

[0051] Example 3

[0052] This embodiment provides a polycrystalline diamond compact, comprising a polycrystalline diamond layer and a cemented carbide substrate. The cemented carbide substrate comprises a 14%wt binder phase comprising 9wt% cobalt and 5wt% chromium, with the remainder being tungsten carbide. The polycrystalline diamond layer and the cemented carbide substrate are sintered under hot-pressing conditions at 1400°C and 7.5 GPa for 10 minutes to produce the polycrystalline diamond compact.

[0053] Example 4

[0054] This embodiment provides a polycrystalline diamond compact, comprising a polycrystalline diamond layer and a cemented carbide substrate. The cemented carbide substrate comprises a 14%wt binder phase comprising 9wt% cobalt, 2.5wt% nickel, and 2.5wt% aluminum, with the remainder being tungsten carbide. The polycrystalline diamond layer and the cemented carbide substrate are sintered under hot-pressing conditions at 1400°C and 7.5 GPa for 10 minutes to produce the polycrystalline diamond compact.

[0055] The polycrystalline diamond compacts prepared in Examples 1-4 were subjected to wear resistance, heat resistance, and impact resistance tests; the final results showed that under the same test conditions, Examples 1-4 had similar wear resistance, heat resistance, and impact resistance.

[0056] Taking into account the working conditions and environment of the drill bit, different tests are conducted on the corrosion resistance of the composite sheet.

[0057] Considering the working state of the drill bit when starting, the corrosion resistance of the polycrystalline diamond compact was tested by oscillating erosion. The oscillating erosion environment was simulated by the combined action of an oscillating motor and a silica gravel suspension.

[0058] Figure 2 is a comparative graph of weight loss after 100 hours of oscillatory erosion for Examples 1, 2, 3, and 4 of the present invention. As shown in Figure 2, under an erosion environment, using weight loss as an indicator of corrosion resistance, Example 1 lost 390 mg during the test at a rate of 3.9 mg / h; Example 2 lost 220 mg during the test at a rate of 2.2 mg / h; Example 3 lost 150 mg during the test at a rate of 1.5 mg / h; and Example 4 lost 180 mg during the test at a rate of 1.8 mg / h. The weight loss rates of Examples 2, 3, and 4 are lower than those of Example 1, indicating that the corrosion resistance is improved at the binder phase ratios of Examples 2, 3, and 4.

[0059] Taking into account the working state of the drill bit when in standby mode, the corrosion resistance of the polycrystalline diamond composite sheet was tested by means of constant temperature corrosion. The constant temperature environment was achieved by a constant temperature water bath at a constant temperature of 80°C.

[0060] FIG3 is a comparative graph of the weight loss of Examples 1, 2, 3, and 4 of the present invention after 100 hours of isothermal corrosion in a salt environment. As shown in FIG3 , in isothermal corrosion, using weight loss as an indicator of corrosion resistance, Example 1 lost 49 mg of weight at a rate of 0.49 mg / h; Example 2 lost 24 mg of weight at a rate of 0.24 mg / h; Example 3 lost 20 mg of weight at a rate of 0.20 mg / h; and Example 4 lost 22 mg of weight at a rate of 0.22 mg / h. The weight loss rates of Examples 2, 3, and 4 are lower than those of Example 1, indicating that the corrosion resistance is improved at the binder phase ratios of Examples 2, 3, and 4.

[0061] Taking into account the working conditions of the drill bit in a more severe environment, the corrosion resistance of the polycrystalline diamond composite sheet was tested by constant temperature corrosion. The constant temperature environment was achieved by a constant temperature water bath with a constant temperature of 80°C and a pH value of 4.0 for the mixed solution.

[0062] Figure 4 is a comparative graph of the weight loss of Examples 1, 2, 3, and 4 of the present invention after 100 hours of isothermal corrosion in a pH 4.0 environment. As shown in Figure 4, weight loss is used as an indicator of corrosion resistance in a pH 4.0 isothermal corrosion environment. Example 1 lost 120 mg of weight during the test at a rate of 1.2 mg / h; Example 2 lost 50 mg of weight during the test at a rate of 0.5 mg / h; Example 3 lost 50 mg of weight during the test at a rate of 0.5 mg / h; and Example 4 lost 70 mg of weight during the test at a rate of 0.7 mg / h. The weight loss rates of Examples 2, 3, and 4 are lower than those of Example 1, indicating that the corrosion resistance is improved at the binder phase ratios of Examples 2, 3, and 4.

[0063] In summary, the present invention provides a cemented carbide substrate, a polycrystalline diamond composite sheet, and a preparation method thereof, wherein the cemented carbide substrate includes a bonding phase and tungsten carbide; the bonding phase includes cobalt and a metal additive; the metal additive is selected from one or more of nickel, chromium, manganese, molybdenum, tin, copper, palladium, silver, aluminum, and platinum. The present invention improves the corrosion resistance of the cemented carbide substrate by introducing specific elements and controlling their proportions to form a corrosion-resistant bonding phase. Since the corrosion-resistant bonding phase changes the corrosion mechanism of the cemented carbide substrate, the corrosion mechanism is more suitable for the use scenario of the polycrystalline diamond composite sheet, thereby effectively improving the corrosion resistance and erosion resistance of the polycrystalline diamond composite sheet, thereby increasing the service life of the composite sheet.

[0064] It should be understood that the application of the present invention is not limited to the above examples. For those skilled in the art, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A cemented carbide substrate, characterized in that: The cemented carbide matrix includes a binder phase and tungsten carbide; the binder phase includes cobalt and metal additives; the metal additives are selected from one or more of nickel, chromium, manganese, molybdenum, tin, copper, palladium, silver, aluminum, and platinum.

2. The cemented carbide substrate according to claim 1, characterized in that: The mass proportion of the binder phase in the cemented carbide matrix is ​​13%-20%.

3. The cemented carbide substrate according to claim 1, characterized in that: The mass of cobalt in the binder phase accounts for 0.5%-16% of the cemented carbide matrix.

4. The cemented carbide substrate according to claim 1, characterized in that: The mass of each metal additive in the binder phase accounts for 0.5%-16% of the cemented carbide matrix.

5. The cemented carbide substrate according to claim 1, characterized in that: The mass of cobalt in the binder phase ranges from 5% to 95%.

6. The cemented carbide substrate according to claim 1, characterized in that The total mass of the metal additives accounts for 5%-95% of the binder phase.

7. A polycrystalline diamond composite sheet, characterized in that: The invention comprises a polycrystalline diamond layer and a cemented carbide substrate as claimed in any one of claims 1 to 6.

8. A method for preparing a polycrystalline diamond compact as claimed in claim 7, characterized in that: Includes steps: Mixing diamond formula powder to obtain mixed powder; placing a cemented carbide substrate on the mixed powder to obtain an assembly block; The assembly block is sintered to obtain a polycrystalline diamond composite sheet.

9. The method for preparing a polycrystalline diamond compact according to claim 8, characterized in that: The temperature of the sintering treatment is 1400-2000° C., the pressure of the sintering treatment is 5-10 GPa, and the time of the sintering treatment is 5-60 minutes.

Citation Information

Patent Citations

  • Polycrystalline diamond compact and preparation method thereof

    CN103072332A

  • Multilayer polycrystalline diamond compact and preparation method thereof

    CN106735246A

  • Polycrystalline Diamond Compact Cutter with Low Cobalt Content Cemented Tungsten Carbide Substrate

    CN110116221A

  • Polycrystalline diamond compact and preparation method thereof

    CN113427006A

  • Polycrystalline diamond compact and preparation method thereof

    CN115555566A